Cartilage extracellular matrix microcapsule, scaffold for tissue engineering, and preparation methods therefor

By using cartilage extracellular matrix microcapsules and high-performance tissue engineering scaffolds, the problem of poor cartilage regeneration and differentiation in the existing technology is solved, effective nutrition and growth of chondrocytes are achieved, and the cartilage damage repair effect is significantly improved. The mechanics of the scaffold Performance and biosafety are superior to natural cartilage.

WO2024198044A1PCT designated stage expired Publication Date: 2024-10-03SUSHENG BIOTECH (HAINAN) CO LTD

Patent Information

Application Number
PCT/CN2023/092630
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2023-05-07
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing tissue engineering scaffolds have poor performance in promoting cartilage regeneration and differentiation, and cannot effectively provide long-term nutrition and growth environment for cartilage seed cells, resulting in poor cartilage damage repair effects.

Method used

Cartilage extracellular matrix microcapsules and tissue engineering scaffolds are used. The microcapsules are composed of chitosan and growth factor TPF-β1/BMP-4 and have a sustained release function. The scaffold has high water absorption and porosity, providing a suitable growth environment. And through specific preparation methods, lipids and heavy metals are removed to ensure biological safety.

Benefits of technology

It achieves long-term nutrient supply and growth of cartilage seed cells, promotes the differentiation of BMSCs into chondrocytes, and significantly improves the regeneration and repair effect of cartilage. The mechanical properties of the scaffold are better than those of natural cartilage, and it has no biological toxicity and is suitable for biological treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023092630_03102024_PF_FP_ABST
    Figure CN2023092630_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the field of tissue engineering. Disclosed are a cartilage extracellular matrix microcapsule, a scaffold for tissue engineering, and preparation methods therefor. The cartilage extracellular matrix microcapsule of the present invention comprises a core material and a wall material wrapping the core material; the mass ratio of the wall material to the core material is preferably 1:(1-3); the wall material is chitosan; the core material comprises a growth factor, an adsorbent, an emulsifier, a dispersant and base oil; and the mass ratio of the growth factor, the adsorbent, the emulsifier, the dispersant and the base oil is (0.01-0.03):(1-10):(1-6):(1-4):(2-6). The scaffold for tissue engineering prepared from the cartilage extracellular matrix microcapsule has excellent mechanical properties, high water absorption, large pore size and no biotoxicity, and not only provides a microenvironment for cells to survive, but also can continuously promote the differentiation and proliferation of BMSCs into chondrocytes, promoting the regeneration and repair of cartilage.
Need to check novelty before this filing date? Find Prior Art

Description

Cartilage extracellular matrix microcapsules, tissue engineering scaffolds and their preparation methods Technical Field

[0001] The present invention belongs to the field of tissue engineering, and in particular relates to a cartilage extracellular matrix microcapsule, a tissue engineering scaffold and a preparation method thereof. Background Art

[0002] Articular cartilage is a hyaline cartilage rich in type II collagen and glycosaminoglycans, which plays a role in bearing mechanical loads and lubricating joints during joint movements. Unlike other tissues, cartilage tissue does not have blood vessels or nerves, and its self-repair ability after degeneration and injury is extremely limited. It is difficult to repair after the damage reaches 3mm, and when the damage reaches 6mm, it will cause damage to the underlying bone. At present, the surgical methods for treating articular cartilage injuries mainly include microfracture, autologous chondrocyte implantation (ACI), mosaicplasty and allogeneic cartilage transplantation. However, these methods all have certain limitations and cannot completely restore the original autologous cartilage. In addition, the prognosis is uncertain. Based on this, the implantation of a suitable tissue engineering scaffold provides a better solution to this problem.

[0003] Cartilage tissue engineering involves culturing and expanding cartilage seed cells in vitro with the presence of factors that promote cell differentiation and proliferation. A certain number of these cells are cultured on a biomaterial scaffold and then transplanted into the cartilage defect site to form new cartilage tissue. This remodeling and integration with the body's tissues results in the regeneration and repair of damaged cartilage. Cartilage tissue engineering primarily involves three aspects: seed cells, biomaterial scaffolds, and growth factors. The biomaterial scaffold, acting as a temporary replacement for the extracellular matrix, provides the three-dimensional geometry of the engineered cartilage tissue and a microenvironment for the seed cells to survive. This provides the basic framework and metabolic space for cell adhesion, proliferation, differentiation, and ultimately the formation of new cartilage tissue, and is therefore crucial to the success of cartilage tissue engineering.

[0004] Currently, the materials used in bioscaffolds mainly include natural and synthetic materials. Synthetic polymers include polyglycolic acid, polylactic acid, polyglycolic acid complexes, and polyvinyl alcohol, while natural polymers include cartilage extracellular matrix, agarose, gelatin, and hyaluronic acid. Among them, cartilage extracellular matrix is ​​widely used as a tissue engineering scaffold material due to its excellent biosafety and biocompatibility, as well as its cell recognition and adhesion sites.

[0005] Existing tissue engineering scaffolds only passively provide a microenvironment for cells to survive, and their performance is relatively poor, and they cannot effectively promote the regeneration and differentiation of cartilage.

[0006] Summary of the Invention

[0007] In view of this, the first purpose of the present invention is to propose a cartilage extracellular matrix microcapsule with a sustained-release function, which can provide nutrition for cartilage seed cells for a long time, maintain the growth of cartilage seed cells in the cartilage defect site, and achieve the regeneration and repair of damaged cartilage.

[0008] The second purpose of the present invention is to provide a method for preparing the above-mentioned cartilage extracellular matrix microcapsules.

[0009] The third purpose of the present invention is to propose a cartilage extracellular matrix tissue engineering scaffold, which has excellent mechanical properties, high water absorption, high pore size, and no biological toxicity. It not only provides a microenvironment for cell survival, but also can continuously promote the differentiation and proliferation of BMSCs into chondrocytes, thereby promoting the regeneration and repair of cartilage.

[0010] The fourth object of the present invention is to provide a method for preparing the above-mentioned cartilage extracellular matrix tissue engineering scaffold.

[0011] The fifth object of the present invention is to provide a mold that can form a stent in a directional manner.

[0012] The cartilage extracellular matrix microcapsules of the present invention include a core material and a wall material wrapped around the core material; the mass ratio of the wall material to the core material is preferably 1:(1-3), more preferably 1:(1-2.5), further preferably 1:(1.2-2), and most preferably 1:(1.4-1.6).

[0013] The wall material of the cartilage extracellular matrix microcapsule provided by the present invention is chitosan; the chitosan has a deacetylation degree of ≥90% and a molecular weight of 20-40w;

[0014] The core material includes growth factor, adsorbent, emulsifier, dispersant and base oil; the mass ratio of the growth factor, adsorbent, emulsifier, dispersant and base oil is (0.01-0.03):(1-10):(1-6):(1-4):(2-6); the most preferred ratio is 0.02:6:3:2:3.

[0015] The growth factors in the core material of the present invention include TPF-β1 and / or BMP-4. Preferably, the growth factors include TPF-β1 and BMP-4, and the two are compounded at a mass ratio of 1:1. The present invention adopts a compounding method of TPF-β1 and BMP-4 to improve the repair of cartilage damage by the scaffold, wherein TPF-β1 can promote the Sox-9 gene expression of bone marrow mesenchymal stem cells and the synthesis of cartilage extracellular matrix, and can promote the metabolism of cartilage cells; BMP-4 can increase the output of extracellular matrix, inhibit cell hypertrophy, and promote stem cells to differentiate into cartilage; however, the production factor is easily inactivated, so a carrier is required to store the growth factor and slowly release it to increase the action time of the growth factor; the ultrastructure of the extracellular matrix is ​​a natural and excellent carrier of growth factors such as TPF-β1 and BMP-4. Using the extracellular matrix as an adsorbent for growth factors can effectively prolong the survival time of the growth factor.

[0016] The adsorbent is cartilage extracellular matrix. Preferably, the particle size of the cartilage extracellular matrix is ​​800-1200 mesh.

[0017] Preferably, the cartilage extracellular matrix of the present invention is derived from bovine, and the method for preparing the cartilage extracellular matrix comprises the following steps:

[0018] S1. Remove the bovine kneecap, open the cavity under sterile conditions, and use a scalpel to remove the cartilage, avoiding the subchondral bone.

[0019] S2. Soak and wash with PBS to remove blood and debris from the cartilage surface;

[0020] S3. Inactivate by soaking in 0.5 mol / L sodium hydroxide solution at a material-liquid ratio of 1:5-1:10, m / V, at 4°C for 24-48 hours;

[0021] S4. Freeze the cartilage in liquid nitrogen and then grind it for 2-4 minutes. Grind it at 1500 rpm for 1-2 minutes.

[0022] S5. Degrease and remove cell membranes, add degreasing solution, the material-liquid ratio is 1:3-1:5, m / V constant temperature oscillation at 37 ° C for 48 hours, and change the solution every 12 hours. The degreasing solution ratio is as follows:

[0023] 3-8 parts of sodium carbonate, 0.1-0.5 parts of EDTA-4Na, 1-3 parts of sodium bicarbonate, 0.5-1 parts of SDS, 0.5-1 parts of triton x-100, 3-5 parts of isopropyl alcohol, 0.1-0.3 parts of AEBSF, and 82.2-92.8 parts of purified water.

[0024] The degreasing solution uses a combination of weakly alkaline sodium carbonate and sodium bicarbonate for degreasing, which can effectively remove lipids from cartilage tissue and is relatively gentle. The added SDS and Triton X-100 can change the permeability of cell membranes, thereby causing cell rupture, and can also increase the solubility of lipids. At the same time, the use of EDTA-4Na as a heavy metal scavenger in the present invention can effectively reduce the heavy metal content in the obtained extracellular matrix, thereby ensuring the biosafety of the extracellular matrix.

[0025] S6. DNase and RNase digestion: Treat the decellularized cartilage tissue with a digestive enzyme mixture containing 50-100 U / ml DNase and 0.5-2 U / ml RNase at a material-to-liquid ratio of 1:1-1:2 (m / v). Digest in a constant temperature shaker at 37°C for 12-24 hours at a frequency of 100-180 rpm.

[0026] S7. repeatedly washing the decellularized cartilage tissue with water and freeze-drying it to obtain a solid cartilage extracellular matrix;

[0027] S8. The solid cartilage extracellular matrix was frozen in liquid nitrogen and then ground for 2-4 minutes. The grinding process was 1500 rpm for 1-2 minutes. After the cartilage extracellular matrix returned to room temperature, it was placed in a 50°C constant temperature drying oven for 0.5-1 hour. The powder below the sieve was first passed through an 800-mesh sieve, and then passed through a 1200-mesh sieve. The powder above the sieve was removed. This process was repeated 3-5 times to obtain the cartilage extracellular matrix powder of the present invention as an adsorbent.

[0028] The cartilage extracellular matrix prepared by the method of the present invention can effectively remove lipids and cells in the cartilage tissue, and can preserve collagen and glycosaminoglycans to a greater extent, maintaining the complete morphology, histology and ultrastructure of the extracellular matrix.

[0029] The emulsifier is Span 80 and / or Span 20.

[0030] The dispersant is preferably polyvinyl alcohol; the alcoholysis degree of the polyvinyl alcohol is preferably 98% to 100%; the viscosity of the polyvinyl alcohol is preferably 5-6 mPa.s; the polyvinyl alcohol preferably has a volatile matter content of ≤5.0, a purity of ≥93.5, and an ash content of ≤0.7; the pH value of the polyvinyl alcohol is preferably 5 to 7; in the present invention, the most preferred polyvinyl alcohol is Aladdin brand, with the product number P139533.

[0031] The base oil is sweet almond oil.

[0032] The preparation method of the cartilage extracellular matrix microcapsules of the present invention comprises:

[0033] S1) Preparation of core material solution: Growth factors and adsorbents are sequentially mixed in PBS to obtain a core material PBS solution; S2) Preparation of oil phase: An emulsifier, a dispersant and sweet almond oil are mixed and heated to obtain an oil phase; S3) Preparation of wall material solution: Chitosan is added to a 0.1 mol / L acetic acid aqueous solution, fully dissolved and filtered to obtain a wall material solution; S4) The core material aqueous solution and the wall material solution are mixed and stirred, and the oil phase is added and continued to stir to obtain a cartilage extracellular matrix microcapsule solution; S5) The cartilage extracellular matrix microcapsule solution is spray-dried to obtain the desired cartilage extracellular matrix microcapsules.

[0034] Specifically, in the above preparation method, the specific operation process of step S1 is as follows: first, the growth factor is added to PBS and stirred. The stirring speed during this process is preferably 500-800 rpm, and the stirring time is preferably 10-30 min, more preferably 15-25 min, and more preferably 20 min; then the adsorbent is slowly added and stirred. The stirring speed during this process is preferably 100-300 rpm; the time is preferably 20-50 min, more preferably 25-40 min, and more preferably 30 min, thereby obtaining a core material PBS solution.

[0035] The emulsifier, dispersant and sweet almond oil are mixed and heated to obtain an oil phase; the temperature of the mixed heating is preferably 50°C to 90°C, more preferably 60°C to 80°C, and more preferably 70°C; the time of the mixed heating is preferably 20 to 50 minutes, more preferably 20 to 40 minutes, and more preferably 30 minutes; the speed of the mixed stirring is preferably 500 to 800 rpm.

[0036] In step S3, chitosan is mixed and stirred with a 0.1 mol / L acetic acid aqueous solution to obtain a wall material solution; the mass ratio of chitosan to acetic acid aqueous solution is preferably 1:(2-5), more preferably 1:(3-4); the rotation speed during the mixing and stirring process is preferably 500-800 rpm; the time is preferably 20-50 min, more preferably 20-40 min, and more preferably 30 min.

[0037] In step S4, when the core material aqueous solution and the wall material solution are mixed and stirred, the mixing and stirring speed is preferably 500-800 rpm, and the mixing and stirring time is preferably 20-50 minutes, more preferably 20-40 minutes, and even more preferably 30 minutes. Then, the oil phase is added and continued stirring to obtain the cartilage extracellular matrix microcapsules. During this process, the stirring speed is preferably 2000-2500 rpm, and the stirring time is preferably 1-4 hours, more preferably 2-3 hours.

[0038] The invention discloses a cartilage extracellular matrix tissue engineering scaffold, which comprises the following raw materials by weight: 0.5-1 parts of cartilage extracellular matrix microcapsules, 0.5-1.5 parts of soluble cartilage extracellular matrix, 0.5-1.5 parts of carboxymethyl chitosan, 0.5-1.5 parts of gelatin, 1-2 parts of hydrochloric acid, 0.05-0.15 parts of inorganic salt, and 92.35-96.95 parts of pure water.

[0039] Among them, cartilage extracellular matrix microcapsules have been introduced in detail above.

[0040] The soluble cartilage extracellular matrix is ​​obtained by further enzymatic hydrolysis of cartilage extracellular matrix powder, and the specific preparation process includes the following steps:

[0041] S1. Prepare a pepsin solution with a pepsin concentration of 0.1-0.3%, and use hydrochloric acid to adjust the pH to 1-3, preferably 1.5-2.5, and most preferably 1.8;

[0042] S2. Thoroughly mix the cartilage extracellular matrix powder and the pepsin solution at a material-liquid ratio of 1:5-1:8, m / V, and oscillate at a constant temperature for 12-24 hours;

[0043] S3, centrifugation and filtration, taking the supernatant, adding 30% hydrogen peroxide solution to terminate the reaction;

[0044] S4. Freeze-drying the solution after the reaction is terminated to obtain the desired soluble extracellular matrix.

[0045] The concentration of the hydrochloric acid is 1 mol / L, and the inorganic salt is one or a mixture of two of sodium chloride, potassium chloride, sodium sulfate, and potassium sulfate.

[0046] The preparation method of the cartilage extracellular matrix tissue engineering scaffold comprises the following steps:

[0047] S1. Preparation of tissue engineering scaffold solution:

[0048] a. Take pure water, add hydrochloric acid and inorganic salt, start stirring, stirring time 10-20min, stirrer speed 300-600r / min;

[0049] b. Add carboxymethyl chitosan and continue stirring for 10-20 min at a stirrer speed of 600-800 r / min;

[0050] c. Add gelatin, raise the temperature to 45-60°C, and continue stirring for 10-20 minutes at a mixer speed of 600-800 rpm;

[0051] d. After cooling naturally to room temperature, add 0.5-1.5 parts of soluble cartilage extracellular matrix and continue stirring for 5-10 minutes at a mixer speed of 300-600 r / min;

[0052] e. Add 0.5-1 parts of cartilage extracellular matrix microcapsules and continue stirring for 5-10 minutes at a mixer speed of 100-200 r / min;

[0053] S2, molding:

[0054] a. Weigh the specified amount of S1 tissue engineering scaffold solution and add it to the mold;

[0055] b. Pre-cool the mold in a 4-6°C refrigerator for 10-20 minutes, then place it in a -20°C refrigerator for 1-2 hours, and finally place it in a -80°C refrigerator for 1-2 hours;

[0056] c. Place the frozen mold into a freeze dryer for freeze drying at -80°C for 12-24 hours;

[0057] S3. Cross-linking: using carbodiimide and succinimide or glutaraldehyde as cross-linking agents, cross-linking at 4°C for 24-48 hours;

[0058] S4. Freeze-drying: The cross-linked scaffold is repeatedly rinsed with purified water. After rinsing, the scaffold is freeze-dried to finally obtain the cartilage extracellular matrix tissue engineering scaffold of the present invention.

[0059] The mold in the present invention includes a bottom plate, a side wall and a top cover, wherein the bottom plate and the top cover are respectively arranged on the upper end opening and the lower end opening of the side wall, wherein the bottom plate is sealed with the side wall, and the top cover is tightly covered on the upper end opening of the side wall, and the bottom plate, the side wall and the top cover form a closed space for accommodating a tissue engineering scaffold solution; the bottom plate is made of a heat-conducting material with a large thermal conductivity coefficient, and the side wall and the top cover are made of a heat-resistant material with a small thermal conductivity coefficient; or, the top cover is made of a heat-conducting material with a large thermal conductivity coefficient, and the side wall and the bottom plate are made of a heat-resistant material with a small thermal conductivity coefficient.

[0060] Preferably, the bottom plate is made of a thermally conductive material with a high thermal conductivity, while the side walls and top cover are made of a heat-resistant material with a low thermal conductivity. Furthermore, the thermal conductivity of the material used to make the top cover is lower than that of the material used to make the side walls. Furthermore, the bottom plate is made of pure copper; the side walls are made of polytetrafluoroethylene; and the top cover is made of fir wood.

[0061] In addition, the bottom plate and the side walls are sealed by bonding with low-temperature resistant glue or by interference fit. A sealing ring is provided at the connection between the top cover and the side walls.

[0062] The side wall is a double-layer hollow structure, which is filled with air or is vacuum.

[0063] The upper bottom surface of the bottom plate is provided with tiny protrusions, and the tiny protrusions are evenly distributed on the bottom surface of the mold bottom plate.

[0064] Compared with the prior art, the present invention has the following beneficial effects:

[0065] The scaffold prepared by the present invention has excellent mechanical properties. The compressive strength of normal human cartilage is 1MPa. The compressive strength of the scaffold prepared by the present invention is better than that of the cartilage itself. Therefore, after implantation into the human body, it can provide better mechanical support. In addition, the water absorption rate of the scaffold of the present invention is very high, which can reach more than 1800%, and the porosity is ≥85%. These properties can provide a very suitable environment for cell growth. At the same time, it can also continuously release growth factors to promote the proliferation and differentiation of bone marrow mesenchymal stem cells. Through testing, it can be seen that the scaffold of the present invention has no biological toxicity and can be used for the treatment of organisms. After treatment, the cartilage grows well and basically completely covers the defect site, with excellent therapeutic effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] FIG1 is a schematic structural diagram of a mold for producing a cartilage extracellular matrix tissue engineering scaffold;

[0067] FIG2 is a schematic diagram of a mold having a base plate with tiny protrusions;

[0068] FIG3 is a photograph of the tissue engineering scaffold product prepared in Example 1;

[0069] FIG4 is a SEM image of the tissue engineering scaffold of Example 1;

[0070] FIG5 is the MTT test results of the tissue engineering scaffold in Example 1;

[0071] FIG6 is a sustained-release curve of the growth factor TFP-β1 in various embodiments;

[0072] FIG7 is a graph showing the recovery of rabbit knee cartilage in the blank control group after 6 weeks of animal experiment;

[0073] Figure 8 shows the recovery of rabbit knee cartilage in the microfracture treatment group after 6 weeks of animal experiment;

[0074] FIG9 is a graph showing cartilage recovery in the rabbit knees after 6 weeks of animal experiment using the engineering scaffold of Example 1. DETAILED DESCRIPTION

[0075] In order to enable those skilled in the art to understand the present invention more clearly and intuitively, the present invention will be further described below with reference to the accompanying drawings.

[0076] The invention discloses a cartilage extracellular matrix tissue engineering scaffold, which comprises the following raw materials by weight: 0.5-1 parts of cartilage extracellular matrix microcapsules, 0.5-1.5 parts of soluble cartilage extracellular matrix, 0.5-1.5 parts of carboxymethyl chitosan, 0.5-1.5 parts of gelatin, 1-2 parts of 1 mol / L hydrochloric acid, 0.05-0.15 parts of inorganic salt, and 92.35-96.95 parts of pure water.

[0077] Among them, the cartilage extracellular matrix microcapsules include a core material and a wall material wrapped around the core material; the mass ratio of the wall material to the core material is preferably 1:(1-3), more preferably 1:(1-2.5), further preferably 1:(1.2-2), and most preferably 1:(1.4-1.6).

[0078] The wall material of the cartilage extracellular matrix microcapsules provided by the present invention is chitosan; the chitosan has a deacetylation degree of ≥90% and a molecular weight of 20-40w; the core material comprises a growth factor, an adsorbent, an emulsifier, a dispersant and a base oil (preferably sweet almond oil); the mass ratio of the growth factor, adsorbent, emulsifier, dispersant and base oil is (0.01-0.03):(1-10):(1-6):(1-4):(2-6); the most preferred ratio is 0.02:6:3:2:3.

[0079] The growth factors in the core material of the present invention include TPF-β1 and / or BMP-4. Preferably, the growth factors include TPF-β1 and BMP-4, and the two are compounded at a mass ratio of 1:1. The present invention adopts a compounding method of TPF-β1 and BMP-4 to improve the repair of cartilage damage by the scaffold, wherein TPF-β1 can promote the Sox-9 gene expression of bone marrow mesenchymal stem cells and the synthesis of cartilage extracellular matrix, and can promote the metabolism of cartilage cells; BMP-4 can increase the output of extracellular matrix, inhibit cell hypertrophy, and promote stem cells to differentiate into cartilage; however, the production factor is easily inactivated, so a carrier is required to store the growth factor and slowly release it to increase the action time of the growth factor; the ultrastructure of the extracellular matrix is ​​a natural and excellent carrier of growth factors such as TPF-β1 and BMP-4. Using the extracellular matrix as an adsorbent for growth factors can effectively prolong the survival time of the growth factor.

[0080] The adsorbent is cartilage extracellular matrix. Preferably, the particle size of the cartilage extracellular matrix is ​​800-1200 mesh.

[0081] Preferably, the cartilage extracellular matrix of the present invention is derived from bovine, and the method for preparing the cartilage extracellular matrix comprises the following steps:

[0082] S1. Remove the bovine kneecap, open the cavity under sterile conditions, and use a scalpel to remove the cartilage, avoiding the subchondral bone.

[0083] S2. Soak and wash with PBS to remove blood and debris from the cartilage surface;

[0084] S3. Inactivate by soaking in 0.5 mol / L sodium hydroxide solution at a material-liquid ratio of 1:5-1:10, m / V, at 4°C for 24-48 hours;

[0085] S4. Freeze the cartilage in liquid nitrogen and then grind it for 2-4 minutes. Grind it at 1500 rpm for 1-2 minutes.

[0086] S5. Degrease and remove cell membranes, add degreasing solution, the material-liquid ratio is 1:3-1:5, m / V constant temperature oscillation at 37 ° C for 48 hours, and change the solution every 12 hours. The degreasing solution ratio is as follows:

[0087] 3-8 parts of sodium carbonate, 0.1-0.5 parts of EDTA-4Na, 1-3 parts of sodium bicarbonate, 0.5-1 parts of SDS, 0.5-1 parts of triton x-100, 3-5 parts of isopropyl alcohol, 0.1-0.3 parts of AEBSF, and 82.2-92.8 parts of purified water.

[0088] The degreasing solution uses a combination of weakly alkaline sodium carbonate and sodium bicarbonate for degreasing, which can effectively remove lipids from cartilage tissue and is relatively gentle. The added SDS and Triton X-100 can change the permeability of cell membranes, thereby rupturing cells and increasing the solubility of lipids. At the same time, EDTA-4Na is used as a heavy metal scavenger in the present invention, which can effectively reduce the heavy metal content in the obtained extracellular matrix and ensure the biosafety of the extracellular matrix.

[0089] S6. DNase and RNase digestion: Treat the decellularized cartilage tissue with a digestive enzyme mixture containing 50-100 U / ml DNase and 0.5-2 U / ml RNase at a material-to-liquid ratio of 1:1-1:2 (m / v). Digest in a constant temperature shaker at 37°C for 12-24 hours at a frequency of 100-180 rpm.

[0090] S7. repeatedly washing the decellularized cartilage tissue with water and freeze-drying it to obtain a solid cartilage extracellular matrix;

[0091] S8. The solid cartilage extracellular matrix was frozen in liquid nitrogen and then ground for 2-4 minutes. The grinding process was 1500 rpm for 1-2 minutes. After the cartilage extracellular matrix returned to room temperature, it was placed in a 50°C constant temperature drying oven for 0.5-1 hour. The powder below the sieve was first passed through an 800-mesh sieve, and then passed through a 1200-mesh sieve. The powder above the sieve was removed. This process was repeated 3-5 times to obtain the cartilage extracellular matrix powder of the present invention as an adsorbent.

[0092] The cartilage extracellular matrix prepared by the method of the present invention can effectively remove lipids and cells in the cartilage tissue, and can preserve collagen and glycosaminoglycans to a greater extent, maintaining the complete morphology, histology and ultrastructure of the extracellular matrix.

[0093] The emulsifier is Span 80 and / or Span 20.

[0094] The dispersant is preferably polyvinyl alcohol; the alcoholysis degree of the polyvinyl alcohol is preferably 98% to 100%; the viscosity of the polyvinyl alcohol is preferably 5-6 mPa.s; the polyvinyl alcohol preferably has a volatile matter content of ≤5.0, a purity of ≥93.5, and an ash content of ≤0.7; the pH value of the polyvinyl alcohol is preferably 5 to 7; in the present invention, the most preferred polyvinyl alcohol is Aladdin brand, with the product number P139533.

[0095] The preparation method of the cartilage extracellular matrix microcapsules of the present invention comprises:

[0096] S1) Preparation of core material solution: Growth factors and adsorbents are sequentially mixed in PBS to obtain a core material PBS solution; S2) Preparation of oil phase: An emulsifier, a dispersant and sweet almond oil are mixed and heated to obtain an oil phase; S3) Preparation of wall material solution: Chitosan is added to a 0.1 mol / L acetic acid aqueous solution, fully dissolved and filtered to obtain a wall material solution; S4) The core material aqueous solution and the wall material solution are mixed and stirred, and the oil phase is added and continued to stir to obtain a cartilage extracellular matrix microcapsule solution; S5) The cartilage extracellular matrix microcapsule solution is spray-dried to obtain the desired cartilage extracellular matrix microcapsules.

[0097] Specifically, in the above preparation method, the specific operation process of step S1 is as follows: first, the growth factor is added to PBS and stirred. The stirring speed during this process is preferably 500-800 rpm, and the stirring time is preferably 10-30 min, more preferably 15-25 min, and more preferably 20 min; then the adsorbent is slowly added and stirred. The stirring speed during this process is preferably 100-300 rpm; the time is preferably 20-50 min, more preferably 25-40 min, and more preferably 30 min, thereby obtaining a core material PBS solution.

[0098] The emulsifier, dispersant and sweet almond oil are mixed and heated to obtain an oil phase; the temperature of the mixed heating is preferably 50°C to 90°C, more preferably 60°C to 80°C, and more preferably 70°C; the time of the mixed heating is preferably 20 to 50 minutes, more preferably 20 to 40 minutes, and more preferably 30 minutes; the speed of the mixed stirring is preferably 500 to 800 rpm.

[0099] In step S3, chitosan is mixed and stirred with a 0.1 mol / L acetic acid aqueous solution to obtain a wall material solution; the mass ratio of chitosan to acetic acid aqueous solution is preferably 1:(2-5), more preferably 1:(3-4); the rotation speed during the mixing and stirring process is preferably 500-800 rpm; the time is preferably 20-50 min, more preferably 20-40 min, and more preferably 30 min.

[0100] In step S4, when the core material aqueous solution and the wall material solution are mixed and stirred, the mixing and stirring speed is preferably 500-800 rpm, and the mixing and stirring time is preferably 20-50 minutes, more preferably 20-40 minutes, and even more preferably 30 minutes. Then, the oil phase is added and continued stirring to obtain the cartilage extracellular matrix microcapsules. During this process, the stirring speed is preferably 2000-2500 rpm, and the stirring time is preferably 1-4 hours, more preferably 2-3 hours.

[0101] The soluble cartilage extracellular matrix is ​​obtained by further enzymatic hydrolysis of the cartilage extracellular matrix, and the specific preparation process includes the following steps:

[0102] S1. Prepare a pepsin solution with a pepsin concentration of 0.1-0.3%, and use hydrochloric acid to adjust the pH to 1-3, preferably 1.5-2.5, and most preferably 1.8;

[0103] S2. Thoroughly mix the cartilage extracellular matrix powder and the pepsin solution at a material-liquid ratio of 1:5-1:8, m / V, and oscillate at a constant temperature for 12-24 hours;

[0104] S3, centrifugation and filtration, taking the supernatant, adding 30% hydrogen peroxide solution to terminate the reaction;

[0105] S4. Freeze-drying the solution after the reaction is terminated to obtain the desired soluble extracellular matrix.

[0106] The concentration of the hydrochloric acid is 1 mol / L, and the inorganic salt is one or a mixture of two of sodium chloride, potassium chloride, sodium sulfate, and potassium sulfate.

[0107] The preparation method of the cartilage extracellular matrix tissue engineering scaffold of the present invention comprises the following steps:

[0108] S1. Preparation of tissue engineering scaffold solution:

[0109] a. Take pure water, add hydrochloric acid and inorganic salt, start stirring, stirring time 10-20min, stirrer speed 300-600r / min;

[0110] b. Add carboxymethyl chitosan and continue stirring for 10-20 min at a stirrer speed of 600-800 r / min;

[0111] c. Add gelatin, raise the temperature to 45-60°C, and continue stirring for 10-20 minutes at a mixer speed of 600-800 rpm;

[0112] d. After cooling naturally to room temperature, add 0.5-1.5 parts of soluble cartilage extracellular matrix and continue stirring for 5-10 minutes at a mixer speed of 300-600 r / min;

[0113] e. Add 0.5-1 parts of cartilage extracellular matrix microcapsules and continue stirring for 5-10 minutes at a mixer speed of 100-200 r / min;

[0114] S2, molding:

[0115] a. Weigh the specified amount of S1 tissue engineering scaffold solution and add it to the mold;

[0116] b. Pre-cool the mold in a 4-6°C refrigerator for 10-20 minutes, then place it in a -20°C refrigerator for 1-2 hours, and finally place it in a -80°C refrigerator for 1-2 hours;

[0117] c. Place the frozen mold into a freeze dryer for freeze drying at -80°C for 12-24 hours;

[0118] S3. Cross-linking: using carbodiimide and succinimide or glutaraldehyde as cross-linking agents, cross-linking at 4°C for 24-48 hours;

[0119] S4. Freeze-drying: The cross-linked scaffold is repeatedly rinsed with purified water. After rinsing, the scaffold is freeze-dried to finally obtain the cartilage extracellular matrix tissue engineering scaffold of the present invention.

[0120] The present application is further described below with reference to Examples 1-5.

[0121] Example 1

[0122] The cartilage extracellular matrix tissue engineering scaffold of this embodiment includes the following components in parts by weight:

[0123] 0.5 parts by weight of cartilage extracellular matrix microcapsules, 1 part by weight of soluble cartilage extracellular matrix, 1 part by weight of carboxymethyl chitosan, 1 part by weight of gelatin, 1 part by weight of 1 mol / L hydrochloric acid, 0.05 parts by weight of inorganic salt (sodium chloride), and 95.45 parts by weight of pure water;

[0124] The preparation method of the cartilage extracellular matrix tissue engineering scaffold comprises the following steps:

[0125] S1. Preparation of tissue engineering scaffold solution: a) Add hydrochloric acid and inorganic salts to pure water, start stirring, and stir for 10 minutes at a speed of 400 r / min; b) Add carboxymethyl chitosan and continue stirring for 10 minutes at a speed of 600 r / min; c) Add gelatin, heat to 50°C, and continue stirring for 20 minutes at a speed of 700 r / min; d) After cooling naturally to room temperature, add soluble cartilage extracellular matrix and continue stirring for 5 minutes at a speed of 400 r / min; e) Add cartilage extracellular matrix microcapsules and continue stirring for 5 minutes at a speed of 100 r / min.

[0126] S2. Molding: a) Add the tissue engineering scaffold solution to the mold; b) Pre-cool the mold in a 4-6°C refrigerator for 20 minutes, then place it in a -20°C refrigerator for 2 hours, and finally place it in a -80°C refrigerator for 1 hour; c) Place the frozen mold in a freeze dryer for freeze drying at -80°C for 24 hours.

[0127] S3, cross-linking: using 50 mM carbodiimide and 10 mM succinimide as cross-linking agents, cross-linking at 4 °C for 24 h;

[0128] S4. Freeze-drying: The cross-linked scaffold is repeatedly rinsed with purified water. After rinsing, the scaffold is freeze-dried to finally obtain the cartilage extracellular matrix tissue engineering scaffold of the present invention.

[0129] The cartilage extracellular matrix microcapsules include a core material and a wall material wrapped around the core material, wherein the mass ratio of the wall material to the core material is preferably 1:1.5; the wall material is chitosan, the chitosan has a deacetylation degree of ≥90% and a molecular weight of 20-40w; the core material includes: a growth factor, an adsorbent, an emulsifier, a dispersant, and a base oil (sweet almond oil); the mass ratio of the growth factor, adsorbent, emulsifier, dispersant, and base oil is 0.02:6:3:2:3;

[0130] The growth factor is TPF-β1 and BMP-4 in a 1:1 ratio; the adsorbent is cartilage extracellular matrix; the cartilage extracellular matrix is ​​derived from cattle, and the particle size of the cartilage extracellular matrix is ​​800-1200 meshes.

[0131] The method for preparing cartilage extracellular matrix as an adsorbent comprises the following steps:

[0132] S1. Take the bovine kneecap, open the cavity under sterile conditions, and use a scalpel to remove the cartilage without removing the subchondral bone.

[0133] S2. Soak and wash with PBS to remove blood and debris from the surface of the cartilage;

[0134] S3, soak inactivated with 0.5 mol / L sodium hydroxide solution, with a solid-liquid ratio of 1:5 m / V, at 4°C for 48 h;

[0135] S4, freezing the cartilage in liquid nitrogen and then grinding it. The freezing time was 3 minutes, and the grinding process was 1500 rpm for 2 minutes.

[0136] S5, remove fat and cell membranes, add degreasing solution, the material-liquid ratio is 1:3, m / V is constantly shaken at 37°C for 48 hours, and the solution is changed every 12 hours; the degreasing solution has the following composition: 5 parts of sodium carbonate, 0.2 parts of EDTA4Na, 2 parts of sodium bicarbonate, 1 part of SDS, 1 part of tritonx-100, 5 parts of isopropanol, 0.1 part of AEBSF, and 85.7 parts of purified water.

[0137] S6, DNase and RNase digestion: The decellularized cartilage tissue was treated with a digestion enzyme mixture containing 50 U / ml DNase and 1 U / ml RNase at a material-to-liquid ratio of 1:1 (m / v). The digestion was carried out in a constant temperature shaker at 37°C for 24 hours with a shaking frequency of 150 rpm.

[0138] S7, repeatedly washing the decellularized cartilage tissue with water, and freeze-drying it to obtain a solid cartilage extracellular matrix;

[0139] S8, the cartilage extracellular matrix of step S7 is cryo-grinded with liquid nitrogen for 3 minutes, the grinding process is 1500 rpm, and the grinding time is 2 minutes. After the cartilage extracellular matrix returns to room temperature, it is placed in a 50°C constant temperature drying oven for 1 hour, first passed through an 800-mesh sieve, and the powder under the sieve is taken. Then, it is passed through a 1200-mesh sieve, and the powder on the sieve is taken. The above operation is repeated 3-5 times to finally obtain the cartilage extracellular matrix powder of the present invention;

[0140] The emulsifier is Span 80 and / or Span 20.

[0141] The dispersant is preferably polyvinyl alcohol; the alcoholysis degree of the polyvinyl alcohol is preferably 98% to 100%; the viscosity of the polyvinyl alcohol is preferably 5-6 mPa·s; the polyvinyl alcohol preferably has a volatile matter content of ≤5.0, a purity of ≥93.5, and an ash content of ≤0.7; the pH value of the polyvinyl alcohol is preferably 5 to 7; in the present invention, the most preferred polyvinyl alcohol is Aladdin's P139533.

[0142] The present invention also provides a method for preparing cartilage extracellular matrix microcapsules, comprising: S1, preparing a core material solution: mixing a growth factor and an adsorbent in PBS to obtain a core material PBS solution; S2, preparing an oil phase: mixing an emulsifier, a dispersant and sweet almond oil and heating them to obtain an oil phase; S3, preparing a wall material solution: adding chitosan to a 0.1 mol / L acetic acid aqueous solution, fully dissolving and filtering to obtain a wall material solution; S4, mixing the core material aqueous solution and the wall material solution, adding the oil phase and continuing to stir to obtain a cartilage extracellular matrix microcapsule solution; S5, spray-drying the cartilage extracellular matrix microcapsule solution to obtain the desired microcapsules.

[0143] In this embodiment, in the above preparation method, the specific operation process of preparing the core material solution is as follows: first, the growth factor is stirred and diluted in PBS to the required content, the stirring speed is preferably 600r / min, and the time is preferably 20min; then the adsorbent is slowly added and stirred, the stirring speed is preferably 100r / min, and the time is preferably 30min to obtain the core material PBS solution.

[0144] During the oil phase preparation process, the temperature for mixing and heating the emulsifier, dispersant and sweet almond oil is preferably 70° C., and the mixing and heating time is preferably 30 minutes; the stirring speed during the mixing process is preferably 800 rpm.

[0145] During the preparation of the wall material solution, the mass ratio of chitosan to acetic acid aqueous solution is preferably 1:(3-4); the rotation speed during the mixing process is preferably 500 rpm, and the mixing time is preferably 30 min.

[0146] The core material aqueous solution and the wall material solution are preferably mixed and stirred at a speed of 500 rpm for 30 min, and then the oil phase is added and the stirring speed is preferably 2500 rpm for 2 h.

[0147] The soluble cartilage extracellular matrix is ​​obtained by further enzymatic hydrolysis of the cartilage extracellular matrix, and the preparation process comprises the following steps:

[0148] S1. Prepare pepsin solution with a pepsin concentration of 0.2% and adjust the pH to 1.8 with hydrochloric acid;

[0149] S2. Thoroughly mix the cartilage extracellular matrix powder and pepsin solution at a material-liquid ratio of 1:5, m / V, and shake at a constant temperature for 24 h;

[0150] S3, centrifugation and filtration, taking the supernatant, adding 30% hydrogen peroxide solution to terminate the reaction;

[0151] S4. Freeze-dry the terminated solution to obtain the desired soluble extracellular matrix.

[0152] The mold structure used in the preparation of the aforementioned cartilage extracellular matrix tissue engineering scaffold is shown in Figure 1, including a bottom plate 1, a side wall 2 and a top cover 3. The bottom plate 1 is arranged on the lower end opening of the side wall 2 and is sealed with the side wall 2. The sealing effect can be achieved by using an interference fit or a low-temperature resistant glue material on the market. The top cover 3 is tightly covered on the upper end opening of the side wall 2. The bottom plate 1, the side wall 2 and the top cover 3 form a closed space for accommodating the tissue engineering scaffold solution.

[0153] To achieve directional solidification in the mold, the base plate 1 is made of a thermally conductive material with a high thermal conductivity coefficient. In this embodiment, pure copper is used, which has excellent thermal conductivity of 386.4 W / (mK). The side walls 2 and top cover 3 are made of heat-resistant materials with low thermal conductivity coefficients. In this embodiment, the side walls 2 are made of acid- and alkali-resistant, highly stable polytetrafluoroethylene (PTFE). Compared to copper, PTFE has a much lower thermal conductivity coefficient of 0.256 W / (mK). The top cover 3 is made of fir wood, which has a thermal conductivity coefficient of 0.09 W / (m·K), effectively blocking cold air from entering the mold.

[0154] During the freezing process of the product, since the side walls 2 and the top cover 3 have excellent heat resistance and the bottom plate 1 has high thermal conductivity, the mold can enable the internal tissue engineering scaffold solution to transfer energy (heat) to the outside world from the bottom in a single direction, and the tissue engineering scaffold solution can only gradually condense into a solid state from the bottom upward, thereby forming a directionally crystallized solid scaffold, and then undergo freeze-drying to form an oriented scaffold.

[0155] In practical applications, a sealing ring can be installed at the connection between the top cover 3 and the side wall 2 to ensure airtightness when the top cover 3 covers the upper opening of the side wall 2. The sealing ring is made of a heat-resistant material. The side wall 2 has a double-layer hollow structure, and the double layer of the side wall 2 is filled with air or a vacuum, which further isolates the side wall 2 from heat and further improves the directional solidification performance of the mold.

[0156] Furthermore, the upper surface of the base plate 2 can be provided with micro-protrusions 4 with a diameter of 100-300 μm and a height of 200 μm. The micro-protrusions 4 are evenly distributed on the upper surface of the mold base plate 2. The presence of the micro-protrusions 4 makes it easier for the tissue engineering scaffold solution to form crystal nuclei at the micro-protrusions, thereby growing upward and forming directional crystals. The micro-protrusions 3 are made of the same material as the base plate 2 and are an integral structure. The mold with the micro-protrusions 4 on the base plate 2 is shown in Figure 2.

[0157] Example 2

[0158] The cartilage extracellular matrix tissue engineering scaffold of this embodiment includes the following components in parts by weight:

[0159] 0.5 parts of cartilage extracellular matrix microcapsules, 0.5 parts of soluble cartilage extracellular matrix, 0.5 parts of carboxymethyl chitosan, 0.5 parts of gelatin, 1 part of 1 mol / L hydrochloric acid, 0.05 parts of inorganic salt (sodium chloride), and 96.95 parts of pure water.

[0160] The preparation method of the cartilage extracellular matrix tissue engineering scaffold in this example is the same as the preparation method of the cartilage extracellular matrix tissue engineering scaffold in Example 1.

[0161] In addition, other aspects, such as the composition and preparation method of the cartilage extracellular matrix microcapsules, the soluble cartilage extracellular matrix, and the selection of materials for each component, remain consistent with those in Example 1.

[0162] Example 3

[0163] The cartilage extracellular matrix tissue engineering scaffold of this embodiment includes the following components in parts by weight:

[0164] 0.5 parts of cartilage extracellular matrix microcapsules, 0.7 parts of soluble cartilage extracellular matrix, 0.8 parts of carboxymethyl chitosan, 0.7 parts of gelatin, 1 part of 1 mol / L hydrochloric acid, 0.05 parts of inorganic salt (sodium chloride), and 96.25 parts of pure water.

[0165] The preparation method of the cartilage extracellular matrix tissue engineering scaffold in this example is the same as the preparation method of the cartilage extracellular matrix tissue engineering scaffold in Example 1.

[0166] In addition, other aspects, such as the composition and preparation method of the cartilage extracellular matrix microcapsules, the soluble cartilage extracellular matrix, and the selection of materials for each component, remain consistent with those in Example 1.

[0167] Example 4

[0168] The cartilage extracellular matrix tissue engineering scaffold of this embodiment includes the following components in parts by weight:

[0169] 0.5 parts of cartilage extracellular matrix microcapsules, 1.2 parts of soluble cartilage extracellular matrix, 1.2 parts of carboxymethyl chitosan, 1.2 parts of gelatin, 1.5 parts of 0.1 mol / L hydrochloric acid, 0.05 parts of inorganic salt (sodium chloride), and 94.35 parts of pure water.

[0170] The preparation method of the cartilage extracellular matrix tissue engineering scaffold in this example is the same as the preparation method of the cartilage extracellular matrix tissue engineering scaffold in Example 1.

[0171] In addition, other aspects, such as the composition and preparation method of the cartilage extracellular matrix microcapsules, the soluble cartilage extracellular matrix, and the selection of materials for each component, remain consistent with those in Example 1.

[0172] Example 5

[0173] The cartilage extracellular matrix tissue engineering scaffold of this embodiment includes the following components in parts by weight:

[0174] 0.8 parts of cartilage extracellular matrix microcapsules, 1 part of soluble cartilage extracellular matrix, 1 part of carboxymethyl chitosan, 1 part of gelatin, 1 part of 1 mol / L hydrochloric acid, 0.05 parts of inorganic salt (sodium chloride), and 95.15 parts of pure water.

[0175] The preparation method of the cartilage extracellular matrix tissue engineering scaffold in this example is the same as the preparation method of the cartilage extracellular matrix tissue engineering scaffold in Example 1.

[0176] In addition, other aspects, such as the composition and preparation method of the cartilage extracellular matrix microcapsules, the soluble cartilage extracellular matrix, and the selection of materials for each component, remain consistent with those in Example 1.

[0177] Taking Example 1 as an example, the appearance of the cartilage extracellular matrix tissue engineering scaffold prepared by the present invention is shown in Figure 3. After observation under a scanning electron microscope, it can be seen that the scaffold has a spatial network structure with a pore size of more than 100 μm and large gaps, which is conducive to the migration and adhesion of cells inside the scaffold, as shown in Figure 4.

[0178] Performance Testing

[0179] Water absorption rate refers to the standard GB / T 1034-2008

[0180] Immerse the sample in 23°C distilled water and place it at the specified temperature for a certain period of time. The mass difference between the beginning of the experiment and after water absorption is measured and expressed as a percentage of the initial mass.

[0181] Calculation formula

[0182] c=(m2-m1) / m1*100

[0183] In the formula

[0184] C—water absorption mass fraction of the sample, expressed in %;

[0185] m1—weight of the sample before immersion and after drying, in mg;

[0186] m2—weight of the sample after immersion, in mg;

[0187] Table 1

[0188] Compression strength refers to the standard GB / T1041-2008

[0189] The calculation formula is: σ=F / A

[0190] Where:

[0191] σ—stress parameter, unit is MPa;

[0192] F—test force, in Newton (N);

[0193] A—Original area of ​​the sample, in square millimeters (mm 2 );

[0194] Table 2

[0195] Porosity reference standard YY / T 1616-2018

[0196] Select a test tube with a scale and fill it with a certain amount of anhydrous ethanol to measure the volume of anhydrous ethanol V1; take 8 stent samples and immerse them fully in anhydrous ethanol, apply negative pressure to suck out the remaining air in the sample, so that the anhydrous ethanol is fully filled in the porous stent and no bubbles escape, and obtain the total volume of the stent and anhydrous ethanol V2; remove the stent soaked with anhydrous ethanol and read the value to obtain the remaining anhydrous ethanol volume V3; test each sample 3 times and take the average value.

[0197] Calculation formula

[0198] E=(V1-V3) / (V2-V3), where:

[0199] V1—initial volume of anhydrous ethanol;

[0200] V2—the volume of anhydrous ethanol in the test tube after the porous support is fully filled with anhydrous ethanol;

[0201] V3—the volume of anhydrous ethanol remaining after the stent filled with anhydrous ethanol is removed;

[0202] Table 3

[0203] The MTT toxicity test uses the MTT method to determine the potential cytotoxicity of the sample, in accordance with GB / T 16886.5-2017, "Biological Evaluation of Medical Devices Part 5: In Vitro Cytotoxicity Tests." This test determines whether the material extract can induce a toxic reaction after contact with cultured cells.

[0204] Evaluation Criteria

[0205] (1) The viability of 50% of the sample extract should be at least equal to or higher than that of 100% of the cells; otherwise, the experiment should be repeated.

[0206] (2) The lower the cell viability %, the greater the potential cytotoxicity.

[0207] (3) The cell viability was less than 70% of the blank group, indicating that the sample had potential cytotoxicity.

[0208] (4) The cell viability percentage of the 100% test sample extract is the final result.

[0209] The test results are shown in Figure 5.

[0210] Growth factor sustained release

[0211] A cartilage extracellular matrix tissue engineering scaffold material with a mass of 0.01 g was added to 1 mL of phosphate buffered saline PBS (pH 7.4), and then shaken at room temperature (20°C to 25°C) with a rotation speed of 80 rpm. After a certain period of sustained release, centrifuge at 10,000 rcf for 5 minutes, take the supernatant and save it, and add an equal amount of fresh PBS buffer (pH 7.4) to continue the sustained release; multiple supernatant samples were taken in this way during the sustained release period. The concentration of growth factor TGF-β1 in the supernatant sample was determined using an ELISA kit, and 3 samples were tested in each group, and the results were averaged. The results are shown in Figure 6, and it can be seen that the sustained release time of the engineering scaffold of the present invention can reach an ultra-long 42 days.

[0212] Small animal experiments

[0213] Test method:

[0214] S1. Induction of anesthesia: New Zealand rabbits were used as experimental animals, and anesthesia was induced by intramuscular injection of xylazine hydrochloride injection;

[0215] S2. Modeling: Use a 4 mm diameter dental drill to drill a cartilage defect model with a diameter of 4 mm and a depth of 2 mm on the femoral cartilage of the knee joint. Rinse the wound with normal saline.

[0216] S3. Treatment: The engineered scaffold of Example 1 was placed in a New Zealand rabbit knee cartilage defect model, sutured, and the recovery was observed. A blank control group without treatment and a microfracture treatment group were also established to compare the joint recovery of the three groups.

[0217] The scaffold prepared by the present invention has excellent mechanical properties. The compressive strength of normal human cartilage is 1MPa. The compressive strength of the scaffold prepared by the present invention is better than that of the cartilage itself. Therefore, after being implanted into the human body, it can provide better mechanical support. Moreover, the water absorption rate of the scaffold of the present invention is very high, which can reach more than 1800%, and the porosity is ≥85%. These properties can provide a very suitable environment for cell growth. At the same time, it can also continuously release growth factors to promote the proliferation and differentiation of bone marrow mesenchymal stem cells. Through the cell growth test, it can be seen that the scaffold of the present invention has no biological toxicity and can be used for the treatment of organisms. It can be seen from Figures 7-9 that without treatment or with microfracture treatment, only fibrocartilage will be formed in the defect area. After treatment with the scaffold of the present invention, the cartilage grows well and basically completely covers the defect area, and the treatment effect is very excellent.

[0218] The above description of the embodiments is intended to facilitate understanding and application of the present invention by those skilled in the art. It will be apparent that those skilled in the art can readily make various modifications to these embodiments and apply the general principles described herein to other embodiments without requiring inventive effort. Therefore, the present invention is not limited to the embodiments described herein, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention should fall within the scope of protection of the present invention.

Claims

1. A cartilage extracellular matrix microcapsule, characterized in that: Including core material and wall material wrapped outside the core material; The mass ratio of the wall material to the core material is preferably 1:(1-3), more preferably 1:(1-2.5), further preferably 1:(1.2-2), and most preferably 1:(1.4-1.6); The wall material is chitosan; The core material includes growth factor, adsorbent, emulsifier, dispersant and base oil; the mass ratio of the growth factor, adsorbent, emulsifier, dispersant and base oil is (0.01-0.03):(1-10):(1-6):(1-4):(2-6); the most preferred ratio is 0.02:6:3:2:

3.

2. The cartilage extracellular matrix microcapsule according to claim 1, characterized in that The growth factors in the core material include TPF-β1 and / or BMP-4. Preferably, the growth factors include TPF-β1 and BMP-4, which are compounded at a mass ratio of 1:

1.

3. The chondrocyte extracellular matrix microcapsule according to claim 1, characterized in that The adsorbent is bovine cartilage extracellular matrix, and the preparation method of the cartilage extracellular matrix comprises the following steps: S1. Take the cow kneecap, open the cavity under sterile conditions, and remove the cartilage using a scalpel; S2. Soak and wash with PBS to remove blood and debris on the surface of the cartilage; S3. Soak in 0.5 mol / L sodium hydroxide solution for inactivation, with a solid-liquid ratio of 1:5-1:10, m / V, at 4°C for 24-48 hours; S4. Freeze the cartilage in liquid nitrogen and then grind it. The freezing time is 2-4 minutes. The grinding process is 1500 rpm and the grinding time is 1-2 minutes. S5. Remove fat and cell membrane, add degreasing solution, the material-liquid ratio is 1:3-1:5, m / V is oscillated at 37°C for 48 hours, and the solution is changed every 12 hours. The degreasing solution has the following composition: 3-8 parts of sodium carbonate, 0.1-0.5 parts of EDTA-4Na, 1-3 parts of sodium bicarbonate, 0.5-1 parts of SDS, 0.5-1 parts of triton x-100, 3-5 parts of isopropanol, 0.1-0.3 parts of AEBSF, and 82.2-92.8 parts of purified water; S6. DNase and RNase digestion: the decellularized cartilage tissue was treated with a digestion enzyme mixture at a solid-liquid ratio of 1:1-1:2, m / V. The digestion enzyme mixture contained 50-100 U / ml DNase and 0.5-2 U / ml RNase. The mixture was placed in a constant temperature shaker at 37°C for 12-24 hours with an oscillation frequency of 100-180 rpm. S7. repeatedly washing the decellularized cartilage tissue with water, freeze-drying it, and obtaining a solid cartilage extracellular matrix; S8. Freeze the solid chondrocyte extracellular matrix with liquid nitrogen and then grind it. The freezing time is 2-4 minutes. The grinding process is 1500 rpm and the grinding time is 1-2 minutes. After the chondrocyte extracellular matrix returns to room temperature, place it in a 50°C constant temperature drying oven for 0.5-1h, first pass it through an 800-mesh sieve, take the powder under the sieve, then pass it through a 1200-mesh sieve, take the powder on the sieve, repeat the above operation 3-5 times to finally obtain the chondrocyte extracellular matrix powder.

4. The cartilage extracellular matrix microcapsule according to claim 1, characterized in that The emulsifier is Span 80 and / or Span 20; The base oil is sweet almond oil; The dispersant is preferably polyvinyl alcohol; the alcoholysis degree of the polyvinyl alcohol is preferably 98% to 100%; the viscosity of the polyvinyl alcohol is preferably 5-6 mPa.s; the polyvinyl alcohol preferably has a volatile matter ≤5.0, a purity ≥93.5, and an ash content ≤0.7; and the pH value of the polyvinyl alcohol is preferably 5 to 7.

5. The method for preparing cartilage extracellular matrix microcapsules according to claim 1, characterized in that: The steps include: S1. Preparation of core material solution: sequentially mixing growth factors and adsorbents in PBS to obtain a core material PBS solution; S2, oil phase preparation: mixing and heating the emulsifier, dispersant and sweet almond oil to obtain an oil phase; S3, wall material solution preparation: chitosan is added into 0.1 mol / L acetic acid aqueous solution, fully dissolved and filtered to obtain a wall material solution; S4, mixing the core material aqueous solution and the wall material solution, adding the oil phase and continuing to stir to obtain a cartilage extracellular matrix microcapsule solution; S5. Spray-drying the chondrocyte extracellular matrix microcapsule solution to obtain the desired chondrocyte extracellular matrix microcapsules.

6. The method for preparing chondrocyte extracellular matrix microcapsules according to claim 5, characterized in that: The specific operation process of step S1 is as follows: first, the growth factor is added to PBS and stirred, and the stirring speed is preferably 500-800 rpm during the process, and the stirring time is preferably 10-30 min, more preferably 15-25 min, and more preferably 20 min; then the adsorbent is slowly added and stirred, and the stirring speed is preferably 100-300 rpm during the process; the time is preferably 20-50 min, more preferably 25-40 min, and more preferably 30 min, so as to obtain a core material PBS solution; In step S2, the emulsifier, dispersant and base oil are mixed and heated to obtain an oil phase; the temperature of the mixed heating is preferably The temperature is preferably 50 to 90°C, more preferably 60 to 80°C, and more preferably 70°C; the mixing and heating time is preferably 20 to 50 min, more preferably 20 to 40 min, and more preferably 30 min; the mixing and stirring speed is preferably 500 to 800 rpm; In step S3, chitosan is mixed with 0.1 mol / L acetic acid aqueous solution to obtain a wall material solution; the mass ratio of chitosan to acetic acid aqueous solution is preferably 1:(2-5), more preferably 1:(3-4); the speed during the mixing and stirring process is preferably 500-800 rpm; the time is preferably 20-50 min, more preferably 20-40 min, and more preferably 30 min; In step S4, when the core material aqueous solution and the wall material solution are mixed and stirred, the mixing and stirring speed is preferably 500-800 rpm, and the time is preferably 20-50 min, more preferably 20-40 min, and more preferably 30 min; then the oil phase is added and continued stirring to obtain cartilage extracellular matrix microcapsules. The stirring speed during this process is preferably 2000-2500 rpm, and the time is preferably 1-4 h, more preferably 2-3 h.

7. A cartilage extracellular matrix tissue engineering scaffold, characterized in that: The invention comprises the following raw materials by weight: 0.5-1 part of the chondrocyte extracellular matrix microcapsules according to any one of claims 1 to 4, 0.5-1.5 parts of soluble chondrocyte extracellular matrix, 0.5-1.5 parts of carboxymethyl chitosan, 0.5-1.5 parts of gelatin, 1-2 parts of hydrochloric acid, 0.05-0.15 parts of inorganic salts, and 92.35-96.95 parts of pure water; the soluble chondrocyte extracellular matrix is ​​obtained by further enzymolysis of bovine chondrocyte extracellular matrix with pepsin solution.

8. The cartilage extracellular matrix tissue engineering scaffold according to claim 7, characterized in that: The preparation process of soluble cartilage extracellular matrix includes the following steps: S1, prepare a pepsin solution, the pepsin concentration is 0.1-0.3%, and use hydrochloric acid to adjust the pH to 1-3, preferably 1.5-2.5, most preferably 1.8; S2. Fully mix the bovine cartilage extracellular matrix powder and the pepsin solution, with a solid-liquid ratio of 1:5-1:8, m / V, and oscillate at a constant temperature for 12-24 hours; S3, centrifugation and filtration, taking the supernatant, adding 30% hydrogen peroxide solution to terminate the reaction; S4. Freeze-drying the solution after the reaction is terminated to obtain the desired soluble extracellular matrix.

9. The cartilage extracellular matrix tissue engineering scaffold according to claim 7, characterized in that: The concentration of the hydrochloric acid is 1 mol / L; The inorganic salt is one or a mixture of sodium chloride, potassium chloride, sodium sulfate, and potassium sulfate.

10. The method for preparing a cartilage extracellular matrix tissue engineering scaffold according to claim 7, characterized in that: The following steps are involved: S1. Preparation of tissue engineering scaffold solution: a. Take pure water, add hydrochloric acid and inorganic salt, start stirring, stirring time 10-20min, stirrer speed 300-600r / min; b. Add carboxymethyl chitosan and continue stirring for 10-20 minutes at a stirring speed of 600-800 r / min; c. Add gelatin, raise the temperature to 45-60°C, continue stirring for 10-20 minutes, and the mixer speed is 600-800r / min; d. After cooling naturally to room temperature, add 0.5-1.5 parts of soluble chondrocyte extracellular matrix and continue stirring for 5-10 minutes at a stirring speed of 300-600 r / min; e. Add 0.5-1 part of chondrocyte extracellular matrix microcapsules and continue stirring for 5-10 minutes at a stirring speed of 100-200 r / min; S2, molding: a. Weigh a specified amount of S1 tissue engineering scaffold solution and add it to the production mold; b. Pre-cool the mold in a 4-6℃ refrigerator for 10-20 minutes, then put it in a -20℃ refrigerator for 1-2 hours, and finally put it in a -80℃ refrigerator for deep cooling for 1-2 hours; c. Place the frozen mold into a freeze dryer for freeze drying at -80°C for 12-24 hours; S3, cross-linking: using carbodiimide and succinimide or glutaraldehyde as cross-linking agents, cross-linking at 4°C for 24-48h; S4, freeze-drying: The cross-linked scaffold is repeatedly rinsed with purified water, and after the rinsing is completed, freeze-dried to finally obtain the cartilage extracellular matrix tissue engineering scaffold of the present invention.

11. A production mold for a cartilage extracellular matrix tissue engineering scaffold according to claim 7, characterized in that: The mold includes a bottom plate, a side wall and a top cover, wherein the bottom plate and the top cover are respectively arranged on the upper end opening and the lower end opening of the side wall, wherein the bottom plate is sealed and connected to the side wall, and the top cover is tightly covered on the upper end opening of the side wall, and the bottom plate, the side wall and the top cover form a closed space for accommodating a tissue engineering scaffold solution; the bottom plate is made of a heat-conducting material with a large thermal conductivity, and the side wall and the top cover are made of a heat-resistant material with a small thermal conductivity; or, the top cover is made of a heat-conducting material with a large thermal conductivity, and the side wall and the bottom plate are made of a heat-resistant material with a small thermal conductivity.

Citation Information

Patent Citations

  • Method for preparing Nabothí»s cyst containing manifold cell growth factors and use thereof

    CN101112365A

  • Preparation method and application for transforming growth factor composite scaffold for in-vivo cartilage repair

    CN102416201A

  • Microencapsulation method for preparing hydrotropic substance serving as core material by using complex coacervation method

    CN102580638A

  • Gel microcapsule with cell recruitment function and preparation method thereof

    CN103169951A

  • Preparation method for biobricks containing mesenchymal stem cell (MSC) and biobrick prepared by using same

    CN106039408A

Cited By

  • Tissue regeneration and repair stent and preparation method thereof

    CN122005940A