Semiconductor device, manufacturing method therefor, and electronic device

By using a self-aligned low-energy ion implantation process in DRAM to dope the electrode areas of silicon semiconductor pillars, the problem of high contact resistance of silicon pillars is solved, device performance is improved, lattice damage is avoided, and efficient doping is achieved Effect.

WO2024198047A1PCT designated stage expired Publication Date: 2024-10-03BEIJING SUPERSTRING ACAD OF MEMORY TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/093288
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2023-05-10
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

In the field of dynamic random access memory (DRAM), the metal-semiconductor contact between the source electrode and drain electrode of the silicon pillar easily forms a Schottky barrier, resulting in high contact resistance. It is difficult for existing technology to effectively reduce the contact resistance and avoid Lattice damage to silicon pillars.

Method used

A self-aligned low-energy ion implantation process is used to dope the electrode area of ​​the silicon semiconductor pillar. By forming a trench on the silicon substrate and performing low-energy ion implantation and annealing diffusion, a high-concentration doping area is formed to avoid doping materials from entering the trench. channel area, reducing contact resistance and improving device performance.

Benefits of technology

It effectively reduces the contact resistance between the source and drain electrodes of silicon semiconductor devices, improves device performance, avoids damage to silicon pillars caused by high-energy injection, eliminates the need for photoresisting plates, and achieves efficient doping effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023093288_03102024_PF_FP_ABST
    Figure CN2023093288_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A semiconductor device, a manufacturing method therefor, and an electronic device, relating to the technical field of semiconductors. The semiconductor device comprises: at least one transistor (10) provided on a substrate (1'), and bit lines (20). The transistor (10) comprises a silicon semiconductor pillar (30) extending in a direction perpendicular to the substrate (1'), and the silicon semiconductor pillar (30) successively comprises a first electrode region (31), a channel region (32) and a second electrode region (33) in a direction approaching the substrate (1'). The bit lines (20) are arranged between the second electrode region (33) and the substrate (1') and are connected to the second electrode region (33). The second electrode region (33) contains a doping material which is used for doping by means of a self-aligned ion implantation process, the average bulk density of the doping material in the second electrode region (33) being greater than or equal to 5e19 atoms / cubic centimeters.
Need to check novelty before this filing date? Find Prior Art

Description

Semiconductor device and manufacturing method thereof, and electronic equipment

[0001] This disclosure claims priority to the Chinese patent application filed with the China Patent Office on March 30, 2023, with application number 202310329995.5 and invention name “Semiconductor device, manufacturing method thereof, and electronic device”, the contents of which should be understood as incorporated into this disclosure by reference. Technical Field

[0002] The embodiments of the present disclosure relate to, but are not limited to, the field of semiconductor technology, and in particular to a semiconductor device and a manufacturing method thereof, and an electronic device. Background Art

[0003] In the field of dynamic random access memory (DRAM), in the manufacturing process of vertical channel transistors using a silicon pillar as the channel, the upper and lower regions of the silicon pillar serve as the source and drain electrodes, respectively, with the middle region serving as the channel. The source electrode on the silicon pillar of the transistor is connected to the metal above it, and the drain electrode on the silicon pillar contacts the metal bit line. The contact between the silicon pillar and the metal is a metal-semiconductor contact, which easily forms a Schottky barrier and results in relatively high contact resistance. Doping is generally required in the source and drain regions of the silicon pillar to reduce the contact resistance with the metal.

[0004] Summary of the Invention

[0005] The following is an overview of the subject matter described in detail herein. This overview is not intended to limit the scope of protection of the present disclosure.

[0006] An embodiment of the present disclosure provides a semiconductor device, comprising: at least one transistor and a bit line arranged on a substrate; the transistor comprises a silicon semiconductor column extending in a direction perpendicular to the substrate, the silicon semiconductor column comprising a first electrode region, a channel region, and a second electrode region in sequence from the top to the direction close to the substrate, the bit line being arranged between the second electrode region and the substrate and connected to the second electrode region; the silicon semiconductor column located in the second electrode region contains an impurity material doped using a self-aligned ion implantation process, the average volume density of the impurity material in the second electrode region being greater than or equal to 5e19 atoms / cubic centimeter; the self-aligned ion implantation process is a self-aligned low-energy ion implantation process.

[0007] In an exemplary embodiment of the present disclosure, the average volume density of the doping material in the second electrode region may be 5e19 atoms / cm 3 to 5e20 atoms / cm 3 .

[0008] In an exemplary embodiment of the present disclosure, the silicon semiconductor pillar located in the first electrode region contains a doping material doped by a self-aligned ion implantation process; the self-aligned ion implantation process is a self-aligned low-energy ion implantation process.

[0009] In an exemplary embodiment of the present disclosure, an implantation energy range of the self-aligned low-energy ion implantation process in the first electrode region and / or the second electrode region may be 5 keV to 100 keV.

[0010] In an exemplary embodiment of the present disclosure, doping may be performed simultaneously on the first electrode region and the second electrode region through a single self-aligned low-energy ion implantation process.

[0011] In an exemplary embodiment of the present disclosure, an average volume density of the doping material in the first electrode region is greater than or equal to 5e19 atoms / cubic centimeter.

[0012] In an exemplary embodiment of the present disclosure, the average volume density of the dopant material in the first electrode region may be 5e19 atoms / cm 3 to 5e20 atoms / cm 3 .

[0013] In an exemplary embodiment of the present disclosure, the semiconductor device may include a plurality of transistors distributed in an array along a first direction and a second direction on the substrate, wherein the first direction intersects the second direction;

[0014] The bit lines may extend along the first direction and be arranged at intervals in the second direction, and the second electrode regions of a row of transistors distributed along the first direction may be connected to the same bit line;

[0015] The transistor may further include: a gate electrode surrounding the channel region and insulated from the channel region; the semiconductor device may further include a plurality of word lines extending along the second direction, the gate electrodes of a column of transistors distributed along the second direction are connected to the same word line, and each gate electrode serves as part of the word line.

[0016] In an exemplary embodiment of the present disclosure, at least the semiconductor located in the channel region of the silicon semiconductor pillar is a single crystal silicon semiconductor, and there are no doped ions in a region of the channel region away from the first electrode region and the second electrode region.

[0017] The present disclosure also provides a method for manufacturing a semiconductor device, wherein the semiconductor device includes at least one transistor and a bit line; the transistor includes a silicon semiconductor column extending in a direction perpendicular to a silicon substrate;

[0018] The method for manufacturing the semiconductor device comprises:

[0019] Forming a silicon semiconductor pillar of each transistor and a trench exposing one side of the silicon semiconductor pillar on the silicon substrate; the trench includes a bottom wall and a side wall, and the silicon semiconductor pillar includes at least a drain region and a channel region to be formed in sequence from the bottom wall of the trench to the opening of the trench;

[0020] Using the opening of the trench as a self-aligned window, a self-aligned ion implantation process is used to perform low-energy ion implantation on the silicon substrate at the bottom wall of the trench, followed by annealing and diffusion to form a doped region located at least in the drain region to be formed between two adjacent silicon semiconductor pillars;

[0021] The average volume density of the ion-implanted doping material in the drain region is greater than or equal to 5e19 atoms / cubic centimeter.

[0022] In an exemplary embodiment of the present disclosure, the self-aligned ion implantation process may be performed before forming the bit line;

[0023] Performing ion implantation on the silicon substrate at the bottom wall of the trench using a self-aligned ion implantation process, and annealing the diffusion process may include:

[0024] depositing a sacrificial oxide layer on the silicon substrate to cover the bottom wall and sidewalls of the trench;

[0025] performing low-energy ion implantation only on the silicon substrate and not on the channel region of the silicon semiconductor pillar using a self-aligned ion implantation process in a direction perpendicular to the silicon substrate, so that doping material is implanted into the silicon substrate exposed by the trench;

[0026] An annealing process is used to diffuse the doping material from the silicon substrate into the drain region of the transistor on both sides of the trench.

[0027] In an exemplary embodiment of the present disclosure, the process of forming the bit line may include:

[0028] After ion implantation is performed on the silicon substrate, etching and removing the sacrificial oxide layer on the bottom wall of the trench so that the trench exposes the silicon substrate;

[0029] Etching the exposed silicon substrate so that the trench extends into the silicon substrate and toward the bottom of the drain region, thereby forming a bit line trench extending along the first direction below the drain regions of a row of silicon semiconductor pillars distributed along a first direction parallel to the silicon substrate;

[0030] The bit line is formed in the bit line trench.

[0031] In an exemplary embodiment of the present disclosure, the self-aligned ion implantation process may be performed after forming the bit line;

[0032] The bit line forming process may include:

[0033] depositing a sacrificial oxide layer on the silicon substrate to cover the bottom wall and sidewalls of the trench;

[0034] Etching and removing the sacrificial oxide layer on the bottom wall of the trench so that the trench exposes the silicon substrate;

[0035] Etching the exposed silicon substrate so that the trench extends into the silicon substrate and toward the bottom of the drain region, thereby forming a bit line trench extending along the first direction below the drain regions of a row of silicon semiconductor pillars distributed along a first direction parallel to the silicon substrate;

[0036] The bit line is formed in the bit line groove, and the bit line is exposed by the trench.

[0037] In an exemplary embodiment of the present disclosure, performing ion implantation on the silicon substrate at the bottom wall of the trench using a self-aligned ion implantation process and then performing annealing diffusion may include:

[0038] Performing ion implantation on the bit line exposed by the trench along a direction perpendicular to the silicon substrate using a self-aligned ion implantation process, so that doping material is implanted into the bit line;

[0039] An annealing process is used to diffuse the dopant material from the bit line into the drain region of the silicon semiconductor pillar.

[0040] In an exemplary embodiment of the present disclosure, the silicon semiconductor pillar may further include a source region, wherein the source region is located on a side of the channel region away from the silicon substrate;

[0041] The method for manufacturing the semiconductor device may further include: performing low-energy ion implantation in the source region using a self-aligned ion implantation process, and annealing and diffusion to form a doped region containing a doping material in the source region.

[0042] In an exemplary embodiment of the present disclosure, the source region and the drain region may be doped simultaneously by a self-aligned ion implantation process, and the doped region of the source region and the doped region of the drain region may be formed simultaneously by an annealing process.

[0043] In an exemplary embodiment of the present disclosure, the implantation depth of the doping material into the silicon substrate may be 0 to 45 nm.

[0044] In an exemplary embodiment of the present disclosure, the implantation depth of the dopant material in the source region may be 0 to 45 nm.

[0045] In an exemplary embodiment of the present disclosure, process conditions of the low-energy ion implantation in the drain region and / or the source region may include an implantation energy of 5 keV to 100 keV.

[0046] In an exemplary embodiment of the present disclosure, the annealing process conditions may include: an annealing temperature of 850° C. to 1100° C., and an annealing time of 5 seconds to 30 seconds.

[0047] An embodiment of the present disclosure further provides an electronic device, which includes the semiconductor device provided by the above embodiment of the present disclosure.

[0048] Other features and advantages of the present disclosure will be described in the following description, and in part will become more apparent from the description, or understood by practicing the present disclosure. The objects and advantages of the present disclosure can be realized and obtained through the structures particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] The accompanying drawings are used to provide an understanding of the technical solution of the present disclosure and constitute a part of the specification. Together with the embodiments of the present disclosure, they are used to explain the technical solution of the present disclosure and do not constitute a limitation to the technical solution of the present disclosure.

[0050] FIG1A is a schematic top view of a semiconductor device according to an exemplary embodiment of the present disclosure;

[0051] FIG1B is a schematic diagram of a longitudinal cross-sectional structure of a local structure of the semiconductor device shown in FIG1 taken along the aa′ direction;

[0052] FIG2 is a process flow chart of a method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure;

[0053] 3 is a schematic diagram of a longitudinal cross-sectional structure in the bb' direction after forming a first trench in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure;

[0054] 4 is a schematic diagram of a longitudinal cross-sectional structure in the bb' direction after depositing an insulating layer in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure;

[0055] 5A is a top view of a method for manufacturing a semiconductor device after forming a second trench according to an exemplary embodiment of the present disclosure;

[0056] FIG5B is a schematic diagram of a longitudinal cross-section of the structure shown in FIG5A along the bb' direction;

[0057] FIG5C is a schematic diagram of a longitudinal cross-section of the structure shown in FIG5A taken along the a-a' direction;

[0058] 6 is a schematic diagram of a longitudinal cross-sectional structure along the aa' direction after depositing a sacrificial oxide layer in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure;

[0059] 7 is a schematic diagram of a longitudinal cross-sectional structure along the aa' direction during ion implantation in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure;

[0060] 8 is a schematic diagram of a longitudinal cross-sectional structure along the aa' direction after forming a doped region in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure;

[0061] 9 is a schematic diagram of a longitudinal cross-sectional structure along the aa' direction after forming a bit line trench according to a method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure;

[0062] 10 is a schematic diagram of a longitudinal cross-sectional structure along the aa' direction after forming a bit line in a method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure;

[0063] 11 is a schematic diagram of a longitudinal cross-sectional structure along the aa′ direction after forming a bit line trench in another method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure;

[0064] 12 is a schematic diagram of a longitudinal cross-sectional structure along the aa' direction after forming a bit line in another method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure;

[0065] 13 is a schematic diagram of a longitudinal cross-sectional structure along the aa' direction of another method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure after a portion of the sacrificial oxide layer is removed;

[0066] 14 is a schematic diagram of a longitudinal cross-sectional structure along the aa' direction during ion implantation in another method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure;

[0067] 15 is a schematic diagram of a longitudinal cross-sectional structure along the aa' direction after forming a doped region in another method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure;

[0068] FIG16 is a distribution diagram of doping materials of source / drain electrodes in the bb' direction obtained by TCAD simulation according to an exemplary embodiment of the present disclosure;

[0069] FIG17 is a doping concentration curve of a doping material of a silicon semiconductor pillar of a semiconductor device obtained according to an exemplary embodiment of the present disclosure;

[0070] FIG18 is a doping concentration curve of the doping material of the silicon semiconductor pillar of the semiconductor device obtained in Examples 2 and 3 of the present disclosure;

[0071] FIG19 is a doping concentration curve of the doping material of the silicon semiconductor pillar of the semiconductor device obtained according to the embodiment of the present disclosure in the absence and presence of backscattering.

[0072] The meanings of the various reference symbols in the accompanying drawings are: 1-silicon substrate; 1'-substrate; 10-transistor; 20-bit line; 21-bit line groove; 30-silicon semiconductor pillar; 31-first electrode region; 32-channel region; 33-second electrode region; 34-doped region; 40-gate electrode; 50-word line; 61-first trench; 62-second trench; 70-insulating layer; 80-sacrificial oxide layer. DETAILED DESCRIPTION

[0073] To make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the embodiments of the present disclosure will be described in detail below with reference to the accompanying drawings. It should be noted that, unless there is a conflict, the embodiments and features in the embodiments of the present disclosure can be combined with each other in any manner.

[0074] The embodiments of the present disclosure are not necessarily limited to the dimensions shown in the drawings, and the shapes and sizes of the components in the drawings do not reflect the true proportions. In addition, the drawings schematically illustrate ideal examples, and the embodiments of the present disclosure are not limited to the shapes or values ​​shown in the drawings.

[0075] In the present disclosure, ordinal numbers such as “first” and “second” are provided to avoid confusion among constituent elements and do not indicate any order, quantity or importance.

[0076] In this disclosure, for convenience, words and phrases indicating orientation or positional relationships, such as "middle," "upper," "lower," "front," "back," "vertical," "horizontal," "top," "bottom," "inside," and "outside," are used to illustrate the positional relationships of constituent elements with reference to the accompanying drawings. This is merely for the convenience of describing this specification and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation. Therefore, it should not be understood as a limitation of this disclosure. The positional relationships of constituent elements may be appropriately changed according to the direction in which each constituent element is described. Therefore, the words and phrases described in this disclosure are not limited and may be appropriately replaced according to the circumstances.

[0077] In this disclosure, unless otherwise expressly specified or limited, the terms "mounted," "connected," and "connected" should be interpreted broadly. For example, they can refer to fixed, removable, or integral connections; mechanical or electrical connections; direct connections, indirect connections through intermediaries, or internal communication between two components. Those skilled in the art will understand the specific meanings of these terms in this disclosure based on the specific circumstances.

[0078] In this disclosure, a transistor refers to an element comprising at least three terminals: a gate electrode, a drain electrode, and a source electrode. A transistor has a channel region between a drain electrode (drain electrode terminal, drain region, or drain electrode) and a source electrode (source electrode terminal, source region, or source electrode), and current can flow through the drain electrode, the channel region, and the source electrode. In this disclosure, the channel region refers to the region through which current primarily flows.

[0079] In the present disclosure, the first electrode region of a silicon semiconductor pillar may serve as the source electrode of a transistor, and the second electrode region may serve as the drain electrode of the transistor, or the first electrode region of a silicon semiconductor pillar may serve as the drain electrode of a transistor, and the second electrode region may serve as the source electrode of the transistor. In cases where transistors with opposite polarities are used or where the direction of current changes during circuit operation, the functions of the "source electrode" and "drain electrode" are sometimes interchanged. Therefore, in the present disclosure, the "source electrode" and "drain electrode" may be interchanged.

[0080] In this disclosure, "electrically connected" includes components connected together via an element having some electrical function. There are no particular limitations on the "element having some electrical function" as long as it enables the transfer of electrical signals between the connected components. Examples of "element having some electrical function" include not only electrodes and wiring, but also switching elements such as transistors, resistors, inductors, capacitors, and other components with various functions.

[0081] In the present disclosure, “parallel” means approximately parallel or almost parallel, for example, a state where the angle formed by two straight lines is greater than -10° and less than 10°, and therefore also includes a state where the angle is greater than -5° and less than 5°.

[0082] In this disclosure, the terms "film" and "layer" may be interchanged. For example, "conductive layer" may be replaced with "conductive film." Similarly, "insulating film" may be replaced with "insulating layer."

[0083] In an embodiment of preparing a vertical transistor using single crystal silicon as a semiconductor channel, the semiconductor channel is a single crystal silicon column having a source region and a drain region at the upper and lower ends and a channel region therebetween. Generally, the source region and the drain region are in contact with metal and are led out of the semiconductor. For example, the drain region is connected to a bit line. Generally, the bit line is a buried bit line at the bottom of the single crystal silicon. The source region and the drain region are the source electrode and the drain electrode, respectively, referred to as source / drain electrodes. In order to eliminate the Schottky barrier between the metal and the source / drain electrodes on the semiconductor column of the transistor, the source / drain electrodes of the transistor can be doped with a high concentration.

[0084] Typically, high-energy ion implantation is used, and the high-energy implantation position is the top of the silicon pillar. The high-energy doping ions pass through the channel region and enter the drain region to be formed at the bottom of the silicon pillar. This step forms the doped source and drain regions while affecting the lattice of the silicon pillar channel region, thereby affecting device performance.

[0085] When manufacturing vertical transistors, the source electrode is at the top, and high-concentration doping of the source electrode is easy to achieve. The drain electrode is at the bottom, and when high-energy doping is performed, the doping material needs to diffuse from the source region through the channel region to the drain region. It can be understood that when high-concentration doping is performed, the doping material must pass through a silicon column of a certain depth to reach the drain electrode at the bottom. High-energy doping can easily cause damage to single-crystalline silicon, especially lattice damage. For example, choosing arsenic as a doping material can easily cause amorphization of single-crystalline silicon columns, resulting in device performance failure; choosing phosphorus with a smaller radius as a doping material, although the damage to silicon is relatively small, the diffusion distance is long, and it is easy to diffuse into the channel region, resulting in reduced device performance. Therefore, bottom doping of vertical transistors is more difficult to achieve.

[0086] In this disclosure, when low-energy ion implantation is used to create the drain region, the implantation location is the trench area between the silicon pillars. Annealing and diffusion are then performed to allow the doped ions to laterally enter the drain region below the channel, effectively reducing or avoiding damage to the channel and improving the doping effect.

[0087] In an exemplary embodiment of the present disclosure, at least the semiconductor located in the channel region of the silicon semiconductor pillar is a single crystal silicon semiconductor, and there are no doped ions in a region of the channel region away from the first electrode region and the second electrode region.

[0088] When low-energy ion implantation is used to create the source region, the implantation location is the top of the silicon pillar. Because low-energy ion implantation eliminates the need to implant ions into the drain region, the ion implantation can be controlled to a certain depth in the silicon pillar, avoiding the channel region. The channel region, near the center or away from the source and drain regions, is devoid of the aforementioned dopant ions. In other words, in a cross-section of the silicon pillar, the center region contains very few or no dopant ions. Furthermore, the semiconductor in this region is single-crystal silicon with a well-defined lattice, not amorphous silicon.

[0089] An embodiment of the present disclosure provides a semiconductor device.

[0090] 1A is a schematic top view of a semiconductor device according to an exemplary embodiment of the present disclosure; FIG. 1B is a schematic longitudinal cross-sectional view of a local structure of the semiconductor device shown in FIG. 1 on the aa′ cross section.

[0091] As shown in Figures 1A and 1B, the semiconductor device includes: at least one transistor 10 and a bit line 20 arranged on a substrate 1'; the transistor 10 includes a silicon semiconductor column 30 extending in a direction perpendicular to the substrate 1', and the silicon semiconductor column 30 includes a first electrode region 31, a channel region 32, and a second electrode region 33 in sequence from the top to the direction close to the substrate 1'; the bit line 20 is arranged between the second electrode region 33 and the substrate 1' and is connected to the second electrode region 33; the second electrode region 33 contains an impurity material doped using a self-aligned low-energy ion implantation process, and the average volume density of the impurity material in the second electrode region 33 is greater than or equal to 5e19 atoms / cubic centimeter.

[0092] The average volume density can be understood as the average value obtained by testing data at multiple locations.

[0093] The source / drain electrodes of the transistors of the semiconductor device of the embodiment of the present disclosure have a high doping concentration and can form ohmic contact with the metal layers above and below the source / drain electrodes. Therefore, the contact resistance between the source / drain electrodes of the transistors and the metal layers is small, and the device performance is better.

[0094] In an exemplary embodiment of the present disclosure, the average volume density of the doping material in the second electrode region 33 may be 5e19 atoms / cm 3 to 5e20 atoms / cm 3 .

[0095] In an exemplary embodiment of the present disclosure, the implantation energy of the self-aligned low-energy ion implantation process may be in a range of 5 keV to 100 keV.

[0096] In an exemplary embodiment of the present disclosure, the doping material may also be doped into the first electrode region through a self-aligned ion implantation process, for example, a self-aligned low-energy ion implantation process.

[0097] In an exemplary embodiment of the present disclosure, an average volume density of the doping material in the first electrode region is greater than or equal to 5e19 atoms / cubic centimeter.

[0098] In an exemplary embodiment of the present disclosure, doping may be performed simultaneously on the first electrode region and the second electrode region through a single self-aligned low-energy ion implantation process.

[0099] In an exemplary embodiment of the present disclosure, the average volume density of the dopant material in the first electrode region may be 5e19 atoms / cm 3 to 5e20 atoms / cm 3 .

[0100] In an exemplary embodiment of the present disclosure, as shown in FIG1A , the semiconductor device may include a plurality of transistors 10. The plurality of transistors 10 may be arranged in an array along a first direction and a second direction on a substrate 1′, wherein the first direction intersects the second direction and the first direction and the second direction may be parallel to the substrate 1′. The first direction may be the a-a′ direction as shown in FIG1A , and the second direction may be the b-b′ direction as shown in FIG1A . A second trench 62 is provided between two adjacent transistors 10 in the first direction, and a first trench 61 is provided between two adjacent transistors 10 in the second direction.

[0101] In an exemplary embodiment of the present disclosure, as shown in FIG. 1A , the bit lines 20 may extend along the first direction and be arranged at intervals in the second direction.

[0102] In an exemplary embodiment of the present disclosure, as shown in FIG. 1B , the second electrode regions 33 of a row of transistors 10 distributed along the first direction may be connected to the same bit line 20 .

[0103] In an exemplary embodiment of the present disclosure, as shown in FIG. 1A , the transistor 10 may further include a gate electrode 40 surrounding the channel region 32 and insulated from the channel region 32 .

[0104] Here, the surrounding can be understood as partial surrounding or full surrounding. In some embodiments, the surrounding can be full surrounding, that is, at least the entire side wall of the channel region 32 is surrounded by the gate electrode 40, and the cross-section of the gate electrode 40 after surrounding is a closed ring. The cross-section is intercepted along the direction perpendicular to the substrate. In some embodiments, the surrounding can be partial surrounding, that is, part of the side wall of the channel region 32 is surrounded by the gate electrode 40, and the cross-section of the gate electrode 40 after surrounding is not closed, but presents a ring shape. For example, a ring with an opening or two independent gate electrodes 40. For example, the opposite side surfaces of the channel region 32 are surrounded by the gate electrode 40, and the cross-section of the gate electrode 40 is a ring with two openings.

[0105] In an exemplary embodiment of the present disclosure, as shown in FIG. 1A , the semiconductor device may further include a plurality of word lines 50 extending along the second direction.

[0106] In an exemplary embodiment of the present disclosure, the gate electrodes 40 of the transistors 10 in a column distributed along the second direction may be connected to the same word line 50 .

[0107] In an exemplary embodiment of the present disclosure, the gate electrodes 40 of a column of transistors 10 distributed along the second direction may be connected to the same word line 50 and serve as a part of the connected word line 50 .

[0108] In an exemplary embodiment of the present disclosure, the transistor may be a vertical gate-all-around (VGAA) transistor; the semiconductor device may be a memory device including a transistor, such as a dynamic random access memory (DRAM), a magnetic random access memory (MRAM), etc.

[0109] The present disclosure also provides a method for manufacturing a semiconductor device, wherein the semiconductor device includes at least one transistor and a bit line; the transistor includes a silicon semiconductor pillar extending in a direction perpendicular to a silicon substrate. The semiconductor device provided in the above embodiment of the present disclosure can be obtained by this manufacturing method.

[0110] FIG. 2 is a process flow chart of a method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure.

[0111] As shown in FIG2 , the method for manufacturing the semiconductor device includes:

[0112] Forming a silicon semiconductor pillar of each transistor and a trench exposing one side of the silicon semiconductor pillar on a silicon substrate; the trench includes a bottom wall and side walls, and the silicon semiconductor pillar includes at least a drain region and a channel region in sequence from the bottom wall of the trench to the opening of the trench, wherein the conductivity of the drain region is higher than that of the channel region;

[0113] Using the opening of the trench as a self-aligned window, a self-aligned ion implantation process is used to perform low-energy ion implantation on the silicon substrate at the bottom wall of the trench, followed by annealing and diffusion to form a doped region located at least in the drain region to be formed between two adjacent silicon semiconductor pillars;

[0114] The average volume density of the ion-implanted doping material in the drain region is greater than or equal to 5e19 atoms / cubic centimeter.

[0115] The manufacturing method of the semiconductor device of the embodiment of the present disclosure uses low-energy ion implantation to achieve high-concentration doping of the drain region of the silicon semiconductor column, which can avoid damage to the silicon semiconductor column caused by high-energy implantation. In addition, the ion doping is performed using a directional self-aligned ion implantation process, which can avoid the doping material from entering the channel region. Therefore, the performance of the semiconductor device obtained is better and no photoresist is required.

[0116] In an exemplary embodiment of the present disclosure, the implantation energy of the low-energy ion implantation in the drain region may be in a range of 5 keV to 100 keV.

[0117] In an exemplary embodiment of the present disclosure, the self-aligned ion implantation process may be performed before forming the bit line;

[0118] Performing ion implantation on the silicon substrate at the bottom wall of the trench using a self-aligned ion implantation process, and annealing the diffusion process may include:

[0119] depositing a sacrificial oxide layer on the silicon substrate to cover the bottom wall and sidewalls of the trench;

[0120] performing low-energy ion implantation only on the silicon substrate and not on the channel region of the silicon semiconductor pillar using a self-aligned ion implantation process in a direction perpendicular to the silicon substrate, so that doping material is implanted into the silicon substrate exposed by the trench;

[0121] An annealing process is used to diffuse the doping material from the silicon substrate into the drain region of the transistor on both sides of the trench.

[0122] In an exemplary embodiment of the present disclosure, the process of forming the bit line may include:

[0123] After ion implantation is performed on the silicon substrate, etching and removing the sacrificial oxide layer on the bottom wall of the trench so that the trench exposes the silicon substrate;

[0124] Etching the exposed silicon substrate so that the trench extends into the silicon substrate and toward the bottom of the drain region, thereby forming a bit line trench extending along the first direction below the drain regions of a row of silicon semiconductor pillars distributed along a first direction parallel to the silicon substrate;

[0125] The bit line is formed in the bit line trench.

[0126] In an exemplary embodiment of the present disclosure, a method for manufacturing a semiconductor device may include:

[0127] forming a silicon semiconductor pillar of each transistor and a trench exposing one side of the silicon semiconductor pillar on a silicon substrate; the trench comprising a bottom wall and side walls, and the silicon semiconductor pillar sequentially comprising a drain region and a channel region to be formed from the bottom wall of the trench to the opening of the trench, wherein the conductivity of the drain region to be formed is higher than that of the channel region;

[0128] depositing a sacrificial oxide layer on the silicon substrate to cover the bottom wall and sidewalls of the trench;

[0129] performing low-energy ion implantation only on the silicon substrate and not on the channel region of the silicon semiconductor pillar using a self-aligned ion implantation process in a direction perpendicular to the silicon substrate, so that doping material is implanted into the silicon substrate exposed by the trench;

[0130] Using an annealing process to diffuse the doping material from the silicon substrate into the drain region of the transistor on both sides of the trench;

[0131] Etching and removing the sacrificial oxide layer on the bottom wall of the trench so that the trench exposes the silicon substrate;

[0132] Etching the exposed silicon substrate so that the trench extends into the silicon substrate and toward the bottom of the drain region, thereby forming a bit line trench extending along the first direction below the drain regions of a row of silicon semiconductor pillars distributed along a first direction parallel to the silicon substrate;

[0133] forming the bit line in the bit line trench;

[0134] The average volume density of the ion-implanted doping material in the second electrode region is greater than or equal to 5e19 atoms / cubic centimeter.

[0135] In an exemplary embodiment of the present disclosure, the self-aligned ion implantation process may be performed after forming the bit line;

[0136] The bit line forming process may include:

[0137] depositing a sacrificial oxide layer on the silicon substrate to cover the bottom wall and sidewalls of the trench;

[0138] Etching and removing the sacrificial oxide layer on the bottom wall of the trench so that the trench exposes the silicon substrate;

[0139] Etching the exposed silicon substrate so that the trench extends into the silicon substrate and toward the bottom of the drain region, thereby forming a bit line trench extending along the first direction below the drain regions of a row of silicon semiconductor pillars distributed along a first direction parallel to the silicon substrate;

[0140] The bit line is formed in the bit line groove, and the bit line is exposed by the trench.

[0141] In an exemplary embodiment of the present disclosure, performing ion implantation on the silicon substrate at the bottom wall of the trench using a self-aligned ion implantation process and then performing annealing diffusion may include:

[0142] Performing ion implantation on the bit line exposed by the trench along a direction perpendicular to the silicon substrate using a self-aligned ion implantation process, so that doping material is implanted into the bit line;

[0143] An annealing process is used to diffuse the dopant material from the bit line into the drain region of the silicon semiconductor pillar.

[0144] In an exemplary embodiment of the present disclosure, a method for manufacturing a semiconductor device may include:

[0145] forming a silicon semiconductor pillar of each transistor and a trench exposing one side of the silicon semiconductor pillar on a silicon substrate; the trench comprising a bottom wall and side walls, and the silicon semiconductor pillar sequentially comprising a drain region and a channel region to be formed from the bottom wall of the trench to the opening of the trench, wherein the conductivity of the drain region to be formed is higher than that of the channel region;

[0146] depositing a sacrificial oxide layer on the silicon substrate to cover the bottom wall and sidewalls of the trench;

[0147] Etching and removing the sacrificial oxide layer on the bottom wall of the trench so that the trench exposes the silicon substrate;

[0148] Etching the exposed silicon substrate so that the trench extends into the silicon substrate and toward the bottom of the drain region, thereby forming a bit line trench extending along the first direction below the drain regions of a row of silicon semiconductor pillars distributed along a first direction parallel to the silicon substrate;

[0149] forming the bit line in the bit line groove, wherein the bit line is exposed by the groove;

[0150] Performing ion implantation on the bit line exposed by the trench along a direction perpendicular to the silicon substrate using a self-aligned ion implantation process, so that doping material is implanted into the bit line;

[0151] Using an annealing process to diffuse the dopant material from the bit line into the drain region of the silicon semiconductor pillar;

[0152] The average volume density of the ion-implanted doping material in the second electrode region is greater than or equal to 5e19 atoms / cubic centimeter.

[0153] In an exemplary embodiment of the present disclosure, the silicon semiconductor pillar may further include a source region, wherein the source region is located on a side of the channel region away from the silicon substrate;

[0154] The method for manufacturing the semiconductor device may further include: performing low-energy ion implantation in the source region using a self-aligned ion implantation process, and annealing and diffusion to form a doped region containing a doping material in the source region.

[0155] In an exemplary embodiment of the present disclosure, the implantation energy of the low-energy ion implantation in the source region may be in a range of 5 keV to 100 keV.

[0156] In an exemplary embodiment of the present disclosure, the source region and the drain region may be doped simultaneously by a self-aligned ion implantation process, and the doped region of the source region and the doped region of the drain region may be formed simultaneously by an annealing process.

[0157] In an exemplary embodiment of the present disclosure, the annealing process conditions may include: an annealing temperature of 850° C. to 1100° C., and an annealing time of 5 seconds to 30 seconds.

[0158] The technical solution of this embodiment is further described below through the manufacturing process of the semiconductor device of this embodiment. Deposition can adopt known processes such as sputtering, evaporation, chemical vapor deposition, coating can adopt known coating processes, and etching can adopt known methods, which are not specifically limited here.

[0159] FIG3 is a schematic diagram of the longitudinal cross-sectional structure of a semiconductor device manufacturing method of an exemplary embodiment of the present disclosure after forming a first trench; FIG4 is a schematic diagram of the longitudinal cross-sectional structure of a semiconductor device manufacturing method of an exemplary embodiment of the present disclosure after depositing an insulating layer in the bb' direction; FIG5A is a top view of the semiconductor device manufacturing method of an exemplary embodiment of the present disclosure after forming a second trench; FIG5B is a schematic diagram of the longitudinal cross-sectional structure of the structure shown in FIG5A in the bb' direction; FIG5C is a schematic diagram of the longitudinal cross-sectional structure of the structure shown in FIG5A in the a-a' direction; FIG6 is a schematic diagram of the longitudinal cross-sectional structure of a semiconductor device manufacturing method of an exemplary embodiment of the present disclosure in the Schematic diagram of the longitudinal cross-sectional structure in the a-a' direction after depositing the sacrificial oxide layer; FIG7 is a schematic diagram of the longitudinal cross-sectional structure in the a-a' direction of a method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure when ion implantation is performed; FIG8 is a schematic diagram of the longitudinal cross-sectional structure in the a-a' direction of a method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure after forming a doped region; FIG9 is a schematic diagram of the longitudinal cross-sectional structure in the a-a' direction of a method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure after forming a bit line groove; FIG10 is a schematic diagram of the longitudinal cross-sectional structure in the a-a' direction of a method for manufacturing a semiconductor device according to an exemplary embodiment of the present disclosure after forming a bit line.

[0160] As shown in FIG. 3 to FIG. 10 , in an exemplary embodiment of the present disclosure, a method for manufacturing a semiconductor device may include:

[0161] S10: Provide a silicon substrate 1, deposit a mask plate on the silicon substrate 1, and form a plurality of first grooves 61 extending along a first direction and spaced apart along a second direction on the silicon substrate 1 through a composition process and an etching process, wherein the first direction and the second direction may be perpendicular to each other; the first grooves 61 expose the silicon substrate 1, and the plurality of first grooves 61 space the upper portion of the silicon substrate 1 into a plurality of semiconductor walls extending along the first direction and spaced apart along the second direction, as shown in FIG3 .

[0162] For example, the silicon substrate may be a single crystal silicon substrate, or a silicon-on-insulator substrate, such as a silicon-on-sapphire (SOS) substrate, a silicon-on-glass (SOG) substrate, or an epitaxial layer of silicon on a base semiconductor. The silicon substrate may be doped or undoped.

[0163] S20 : ​​depositing an insulating layer 70 covering the first trench 61 on the silicon substrate 1 , and planarizing the insulating layer 70 by chemical mechanical polishing (CMP) and removing the insulating layer 70 on the top surface of the semiconductor wall, as shown in FIG. 4 .

[0164] Exemplarily, the insulating layer may be a silicon oxide (SiOx) layer, or a low-K dielectric layer, i.e., a dielectric layer with a dielectric constant K < 3.9. For example, it may be any one or more of silicon nitride (SiNx), silicon oxynitride (SiON), and silicon carbide (SiC).

[0165] S30: Etching on the silicon substrate 1 to form a plurality of second trenches 62 extending along the second direction and spaced apart along the first direction; the plurality of second trenches 62 separate the upper portion of the silicon substrate 1 into a plurality of silicon semiconductor pillars 30 spaced apart and distributed in an array along the first direction and the second direction, and the second trenches 62 expose the side walls of the silicon substrate 1 and the silicon semiconductor pillars 30; the second trench 62 includes a bottom wall and side walls, and from the bottom wall of the second trench 62 to the opening direction of the second trench 62, the silicon semiconductor pillar 30 includes a second electrode region 33, a channel region 32 and a first electrode region 31 in sequence, wherein the first electrode region 31 is a source region and the second electrode region 33 is a drain region, as shown in Figures 5A to 5C; here, the longitudinal section in Figure 5C is perpendicular to the silicon substrate and does not pass through the silicon semiconductor pillars.

[0166] S40 : depositing a sacrificial oxide layer 80 on the silicon substrate 1 to cover the end surface of the first electrode region 31 , the bottom wall and the sidewalls of the second trench 62 . The sidewalls of the silicon semiconductor pillar 30 are also covered by the sacrificial oxide layer 80 , as shown in FIG6 .

[0167] There are gaps in the crystal lattice of single crystal silicon, etc. The function of the sacrificial oxide layer 80 is to prevent the energetically injected ions from damaging the crystal lattice of the single crystal silicon, etc. below during ion implantation, thereby protecting the crystal lattice.

[0168] S50: Using the top surface of the first electrode region 31 and the opening of the second trench 62 as self-aligned windows, a single self-aligned ion implantation process is used to simultaneously perform low-energy ion implantation (implant doping) on ​​the end surface of the first electrode region 31 and the bottom wall of the second trench 62 in a direction perpendicular to the silicon substrate 1, so that doping material is simultaneously implanted into the silicon substrate 1 below the first electrode region 31 and the second trench 62, as shown in FIG7 . The arrows in FIG7 indicate the direction of the self-aligned ion implantation, i.e., a direction perpendicular to the silicon substrate 1 (with an angle of 0° with the silicon semiconductor pillar 30), so that ion implantation is not performed on the channel region of the silicon semiconductor pillar. Among them, the energy of low-energy ion implantation is 5kev to 100kev; the implantation depth of the doping material in the first electrode region 31, that is, after the ion implantation is completed, the distance between the position of the doping material in the first electrode region 31 and the top surface of the first electrode region 31, can be 0 to 45nm; the implantation depth of the doping material in the silicon substrate 1, that is, after the ion implantation is completed, the distance between the position of the doping material in the silicon substrate 1 and the bottom wall of the second trench 62, can be 0 to 45nm.

[0169] The solution of this embodiment uses low-energy ion implantation to achieve high-concentration doping of the first electrode region and the second electrode region of the silicon semiconductor column, which can avoid damage to the silicon semiconductor column caused by high-energy implantation. In addition, the ion doping is performed using a directional self-aligned ion implantation process, which can avoid the doping material from entering the channel region. Therefore, the performance of the semiconductor device produced is better and no photoresist is required.

[0170] For example, for N-type metal-oxide-semiconductor (NMOS) transistors, the doping material may include, but is not limited to, any one or more of phosphorus (P) and arsenic (As); for P-type metal-oxide-semiconductor (NMOS) transistors, the doping material may include, but is not limited to, any one or more of boron (B) and gallium (Ga). The doping depth and doping concentration of the doping material can be adjusted according to actual needs.

[0171] S60: An annealing process is used to diffuse the doping material in the first electrode region 31, and the doping material is diffused from the silicon substrate 1 into the second electrode region 33, forming a doping region 34 in the first electrode region 31 and the second electrode region 33, as shown in Figure 8; wherein, the average volume density of the ion-implanted doping material in the first electrode region 31 is greater than or equal to 5e19 atoms / cubic centimeter, and the average volume density of the ion-implanted doping material in the second electrode region 33 is greater than or equal to 5e19 atoms / cubic centimeter; the doping material is basically uniformly distributed in the first electrode region 31, and the doping material is basically uniformly distributed in the second electrode region 33.

[0172] For example, the annealing process may be thermal annealing or spike annealing, which can activate ions and expand the ion diffusion region. The annealing temperature may be 850° C. to 1100° C., and the annealing time may be 5 seconds to 30 seconds.

[0173] S70: etching away the sacrificial oxide layer 80 on the bottom wall of the second trench 62, so that the second trench 62 exposes the silicon substrate 1; etching the exposed silicon substrate 1 so that the second trench 62 extends into the silicon substrate 1 and extends toward the bottom end of the second electrode region 33, forming a bit line trench 21 extending along the first direction below the second electrode region 33 of a row of silicon semiconductor pillars 30 distributed along the first direction, as shown in FIG9;

[0174] S80 : depositing a conductive layer in the bit line trench 21 to form the bit line 20 , as shown in FIG. 10 .

[0175] Exemplarily, the deposition of the conductive layer may include: depositing a first metal layer on the inner wall of the bit line trench 21, then performing rapid thermal annealing (RTA) to react silicon in the silicon substrate with a first metal in the first metal layer to form a silicide of the first metal, and then using a second metal layer to fill the bit line trench 21. The first metal may include, but is not limited to, at least one of cobalt (Co) and titanium (Ti), and the second metal may be tungsten (W), etc.

[0176] For example, the depth of the first trench 61 is greater than the depth of the second trench 62 , and two adjacent bit lines 20 may be insulated from each other by an insulating layer deposited at the bottom of the first trench 61 .

[0177] Figure 11 is a schematic diagram of the longitudinal cross-sectional structure of another semiconductor device manufacturing method according to an exemplary embodiment of the present disclosure in the a-a' direction after forming a bit line groove; Figure 12 is a schematic diagram of the longitudinal cross-sectional structure of another semiconductor device manufacturing method according to an exemplary embodiment of the present disclosure in the a-a' direction after forming a bit line; Figure 13 is a schematic diagram of the longitudinal cross-sectional structure of another semiconductor device manufacturing method according to an exemplary embodiment of the present disclosure in the a-a' direction after removing part of the sacrificial oxide layer; Figure 14 is a schematic diagram of the longitudinal cross-sectional structure of another semiconductor device manufacturing method according to an exemplary embodiment of the present disclosure in the a-a' direction when performing ion implantation; Figure 15 is a schematic diagram of the longitudinal cross-sectional structure of another semiconductor device manufacturing method according to an exemplary embodiment of the present disclosure in the a-a' direction after forming a doped region.

[0178] As shown in FIG3 to FIG6 and FIG11 to FIG15, in another exemplary embodiment of the present disclosure, the method for manufacturing a semiconductor device may include:

[0179] Steps S10' to S40' are substantially the same as steps S10 to S40 of the above embodiment, except that in step S20', the insulating layer 70 on the top surface of the semiconductor wall is not removed during CMP, and the insulating layer 70 with a thickness of about 5 nm to 10 nm is retained.

[0180] S50': The sacrificial oxide layer 80 on the bottom wall of the second trench 62 is etched away, so that the second trench 62 exposes the silicon substrate 1; the sacrificial oxide layer 80 on the side wall of the second trench 62 is used as a barrier layer to etch the exposed silicon substrate 1, so that the second trench 62 extends into the silicon substrate 1 and extends toward the bottom end of the second electrode region 33, and a bit line groove 21 extending along the first direction is formed below the second electrode region 33 of a column of silicon semiconductor pillars 30 distributed along the first direction, as shown in Figure 11.

[0181] S60 ′: depositing a conductive layer in the bit line groove 21 to form the bit line 20 . The bit line 20 is exposed by the second trench 62 , as shown in FIG. 12 .

[0182] S70': The sacrificial oxide layer 80 on the sidewall of the second trench 62 is etched away. The sacrificial oxide layer 80 on the end surface of the first electrode region 31 of the silicon semiconductor column 30 can be removed together. Subsequently, an insulating layer 70 of a suitable material is used as the sacrificial oxide layer, as shown in FIG13 . Alternatively, the sacrificial oxide layer 80 on the end surface of the first electrode region 31 of the silicon semiconductor column 30 is retained at a certain thickness.

[0183] S80': Using the top surface of the first electrode region 31 and the opening of the second trench 62 as self-aligned windows, a single self-aligned low-energy ion implantation process is used to simultaneously implant ions into the end surface of the first electrode region 31 and the bit line 20 exposed by the second trench 62, along a direction perpendicular to the silicon substrate 1. This allows dopant material to be implanted into both the first electrode region 31 and the bit line 20, as shown in FIG14 . The arrows in FIG14 indicate the direction of the self-aligned ion implantation, i.e., a direction perpendicular to the silicon substrate 1 (with an angle of 0° with the silicon semiconductor pillar 30). The low-energy ion implantation energy is 5 keV to 100 keV. The implantation depth of the dopant material in the first electrode region 31, i.e., the distance from the position of the dopant material in the first electrode region 31 to the top surface of the first electrode region 31 after the ion implantation is completed, can be 0 to 45 nm. The implantation depth of the dopant material in the silicon substrate 1, i.e., the distance from the position of the dopant material in the silicon substrate 1 to the bottom wall of the second trench 62 after the ion implantation is completed, can be 0 to 45 nm.

[0184] S90': An annealing process is performed to diffuse the dopant material into the first electrode region 31. The dopant material is then diffused from the bit line 20 into the second electrode region 33, forming a doped region 34 in the first electrode region 31 and the second electrode region 33, as shown in FIG15 . The average volume density of the ion-implanted dopant material in the first electrode region 31 and the second electrode region 33 is greater than or equal to 5e19 atoms / cm3. Arsenic (As) plasma can enter the second electrode region 33 through lateral straggling.

[0185] In an exemplary embodiment of the present disclosure, the methods of forming the first trench and the second trench may be independently selected from any one or more of dry etching and wet etching.

[0186] In an exemplary embodiment of the present disclosure, the bit line trench may be formed by side-etching the lower portion of the second trench using any one or more of dry etching and wet etching.

[0187] In an exemplary embodiment of the present disclosure, the method of depositing the insulating layer may be selected from any one of atomic layer deposition (ALD) and chemical vapor deposition (CVD).

[0188] In an exemplary embodiment of the present disclosure, the sacrificial oxide layer may be deposited by atomic layer deposition (ALD).

[0189] In an exemplary embodiment of the present disclosure, the method for manufacturing the semiconductor device may further include: etching and removing the insulating layer and the sacrificial oxide layer on the side walls of the channel region of the silicon semiconductor column, sequentially depositing a gate insulating layer and a gate electrode surrounding the side walls of the channel region on the side walls of the channel region, and connecting the gate electrode to the word line.

[0190] In an exemplary embodiment of the present disclosure, the material of the gate insulating layer may be selected from any one or more of silicon oxide (e.g., SiO2), hafnium oxide (e.g., HfO2), zirconium oxide (e.g., ZrO), and aluminum oxide (e.g., Al2O3). The gate insulating layer may be a single-layer structure or a multi-layer structure. For example, it may include a two-layer structure formed by silicon oxide and hafnium oxide, wherein the silicon oxide layer is in contact with the channel region and the hafnium oxide layer is in contact with the gate. The thickness of the gate insulating layer may be set according to actual electrical requirements, for example, it may be 2 nm to 5 nm.

[0191] According to TCAD (Technology Computer Aided Design) simulation, the manufacturing method of the above-mentioned semiconductor device provided in the embodiment of the present disclosure can make the average volume density of the doping material in the first electrode region 31 greater than or equal to 5e19 atoms / cubic centimeter, and the average volume density in the second electrode region 33 greater than or equal to 5e19 atoms / cubic centimeter. Therefore, the manufacturing method of the above-mentioned semiconductor device provided in the embodiment of the present disclosure is feasible.

[0192] The feasibility of the disclosed solution is illustrated below through several TCAD simulation examples.

[0193] Example 1

[0194] In the method for manufacturing a semiconductor device according to the exemplary embodiment of the present disclosure, after the ion implantation of the source / drain electrodes is completed, a simulation is performed using TCAD; wherein,

[0195] The doping material in the channel region is As, the ion implantation energy is 60kev to 180kev, and the average volume density of the doping material in the channel region is 5e12 atoms / cm3 to 8e13 atoms / cm3; the annealing temperature is 850°C to 1100°C, and the annealing time is 5s to 30s;

[0196] The doping material of the source / drain electrode is As, the energy of the low-energy ion implantation is 15kev to 50kev, the doping concentration is 2e14 atoms / cubic centimeter to 3e15 atoms / cubic centimeter; the annealing temperature is 850°C to 1100°C, and the annealing time is 5s to 30s.

[0197] The simulation results are shown in Figures 16 and 17. Figure 16 shows the distribution of the dopant material of the source / drain electrodes in the bb' direction obtained using TCAD simulation for an exemplary embodiment of the present disclosure; Figure 17 shows the dopant concentration curve of the dopant material of the silicon semiconductor pillar of the semiconductor device obtained for an exemplary embodiment of the present disclosure, where the horizontal axis represents the depth from the upper surface (source electrode end surface) of the silicon semiconductor pillar to the interior of the silicon semiconductor pillar.

[0198] Example 2

[0199] In the method for manufacturing a semiconductor device of the exemplary embodiment of the present disclosure, the doping material of the channel region is As, the ion implantation energy is 60kev to 180kev, and the doping concentration is 5e12 atoms / cm3 to 8e13 atoms / cm3;

[0200] The doping material of the source / drain electrode is As, the energy of the low-energy ion implantation is 15kev to 50kev, and the doping concentration is 2e14 atoms / cubic centimeter to 3e15 atoms / cubic centimeter.

[0201] Example 3

[0202] In the method for manufacturing a semiconductor device of the exemplary embodiment of the present disclosure, the doping material of the channel region is As, the ion implantation energy is 60kev to 180kev, and the doping concentration is 5e12 atoms / cm3 to 8e13 atoms / cm3;

[0203] The doping material of the source / drain electrode is P, the energy of the low-energy ion implantation is 5kev to 20kev, and the doping concentration is 5e14 atoms / cubic centimeter to 5e15 atoms / cubic centimeter.

[0204] 18 is a doping concentration curve of the doping material of the silicon semiconductor column of the semiconductor device obtained in Examples 2 and 3 of the present disclosure, wherein the horizontal axis is the depth from the upper surface (source electrode end surface) of the silicon semiconductor column to the interior of the silicon semiconductor column.

[0205] Figure 19 shows the doping concentration curves of the dopant material of the silicon semiconductor pillar of the semiconductor device obtained in the embodiment of the present disclosure, respectively, without and with backscattering. The horizontal axis represents the depth from the top surface (source electrode end surface) of the silicon semiconductor pillar to the interior of the silicon semiconductor pillar. (Based on Figure 19, the backscattering dose can be assumed to be negligible.)

[0206] It can be seen that the manufacturing method of the semiconductor device provided by the embodiment of the present disclosure can achieve high-concentration doping of the source / drain electrodes of the transistor, so that the doping concentration of the source / drain electrodes is much higher than the doping concentration of the channel region.

[0207] An embodiment of the present disclosure further provides an electronic device, which includes the semiconductor device provided by the above embodiment of the present disclosure.

[0208] In exemplary embodiments of the present disclosure, the electronic device may be a storage device, a smart phone, a computer, a tablet, an artificial intelligence device, a wearable device, or a mobile power supply, etc. The storage device may include a memory in a computer, etc., which is not limited here.

[0209] Although the embodiments disclosed in this disclosure are as described above, the contents described are merely embodiments adopted to facilitate understanding of the disclosure and are not intended to limit the disclosure. Any person skilled in the art to which the disclosure belongs may make any modifications and changes in the form and details of the implementation without departing from the spirit and scope of the disclosure. However, the scope of protection of the disclosure shall still be based on the scope defined by the appended claims.

Claims

1. A semiconductor device, comprising: At least one transistor and a bit line are arranged on a substrate; the transistor includes a silicon semiconductor column extending in a direction perpendicular to the substrate, the silicon semiconductor column includes a first electrode region, a channel region and a second electrode region in sequence from the top to the direction close to the substrate, the bit line is arranged between the second electrode region and the substrate and connected to the second electrode region; the silicon semiconductor column located in the second electrode region contains an impurity material doped by a self-aligned ion implantation process, and the average volume density of the impurity material in the second electrode region is greater than or equal to 5e19 atoms / cubic centimeter; the self-aligned ion implantation process is a self-aligned low-energy ion implantation process.

2. The semiconductor device according to claim 1, wherein The average volume density of the doping material in the second electrode region is 5e19 atoms / cubic centimeter to 5e20 atoms / cubic centimeter.

3. The semiconductor device according to claim 1, wherein The silicon semiconductor column located in the first electrode region contains a doping material doped by a self-aligned ion implantation process; the self-aligned ion implantation process is a self-aligned low-energy ion implantation process.

4. The semiconductor device according to claim 1 or 3, wherein: The implantation energy of the self-aligned low-energy ion implantation process in the first electrode region and / or the second electrode region is in a range of 5 keV to 100 keV.

5. The semiconductor device according to claim 4, wherein: Doping is performed simultaneously in the first electrode region and the second electrode region through a self-aligned low-energy ion implantation process.

6. The semiconductor device according to claim 3, wherein: The average volume density of the doping material in the first electrode region is greater than or equal to 5e19 atoms / cubic centimeter.

7. The semiconductor device according to claim 6, wherein: The average volume density of the doping material in the first electrode region is 5e19 atoms / cubic centimeter to 5e20 atoms / cubic centimeter.

8. The semiconductor device according to any one of claims 1 to 7, comprising a plurality of transistors distributed in an array along a first direction and a second direction on the substrate, wherein the first direction intersects the second direction; The bit lines extend along the first direction and are arranged at intervals in the second direction, and the second electrode regions of a row of transistors distributed along the first direction are connected to the same bit line; The transistor further comprises: A gate electrode surrounds the channel region and is insulated from the channel region; the semiconductor device also includes a plurality of word lines extending along the second direction, the gate electrodes of a column of transistors distributed along the second direction are connected to the same word line, and each gate electrode serves as a part of the word line.

9. The semiconductor device according to any one of claims 1 to 8, wherein: At least the semiconductor in the channel region of the silicon semiconductor column is a single crystal silicon semiconductor, and there are no doped ions in a region of the channel region away from the first electrode region and the second electrode region.

10. A method for manufacturing a semiconductor device, wherein: The semiconductor device includes at least one transistor, a bit line; The transistor includes a silicon semiconductor pillar extending in a direction perpendicular to the silicon substrate; The method for manufacturing the semiconductor device comprises: Forming a silicon semiconductor column of each transistor and a trench exposing one side of the silicon semiconductor column on the silicon substrate; the trench comprises a bottom wall and a side wall, and from the bottom wall of the trench to the opening direction of the trench, the silicon semiconductor column at least comprises a drain region and a channel region to be formed in sequence; Using the opening of the trench as a self-aligned window, a self-aligned ion implantation process is used to perform low-energy ion implantation on the silicon substrate at the bottom wall of the trench, and annealing and diffusion are performed to form a doped region of the drain region to be formed at least in two adjacent silicon semiconductor pillars; The average volume density of the ion-implanted doping material in the drain region is greater than or equal to 5e19 atoms / cubic centimeter.

11. The method for manufacturing a semiconductor device according to claim 10, wherein: The self-aligned ion implantation process is performed before forming the bit line; The process of implanting ions into the silicon substrate at the bottom wall of the trench by a self-aligned ion implantation process and annealing and diffusing the ions comprises: Depositing a sacrificial oxide layer covering the bottom wall and sidewalls of the trench on the silicon substrate; In a direction perpendicular to the silicon substrate, a self-aligned ion implantation process is used to perform low-energy ion implantation only on the silicon substrate but not on the channel region of the silicon semiconductor column, so that doping material is implanted into the silicon substrate exposed by the groove; An annealing process is used to diffuse the doping material from the silicon substrate into the drain region of the transistor on both sides of the trench.

12. The method for manufacturing a semiconductor device according to claim 11, wherein: The bit line forming process includes: After ion implantation is performed on the silicon substrate, etching and removing the sacrificial oxide layer on the bottom wall of the trench so that the trench exposes the silicon substrate; Etching the exposed silicon substrate so that the trench extends into the silicon substrate and toward the bottom of the drain region, and forming a bit line groove extending along the first direction below the drain region of a row of silicon semiconductor pillars distributed along a first direction parallel to the silicon substrate; The bit line is formed in the bit line groove.

13. The method for manufacturing a semiconductor device according to claim 10, wherein: The self-aligned ion implantation process is performed after forming the bit line; The bit line forming process includes: Depositing a sacrificial oxide layer covering the bottom wall and sidewalls of the trench on the silicon substrate; Etching and removing the sacrificial oxide layer on the bottom wall of the trench so that the trench exposes the silicon substrate; Etching the exposed silicon substrate so that the trench extends into the silicon substrate and toward the bottom of the drain region, and forming a bit line groove extending along the first direction below the drain region of a row of silicon semiconductor pillars distributed along a first direction parallel to the silicon substrate; The bit line is formed in the bit line groove, and the bit line is exposed by the trench.

14. The method for manufacturing a semiconductor device according to claim 13, wherein: The process of implanting ions into the silicon substrate at the bottom wall of the trench by a self-aligned ion implantation process and annealing and diffusing the ions comprises: Performing ion implantation on the bit line exposed by the trench along a direction perpendicular to the silicon substrate by using a self-aligned ion implantation process, so that doping material is implanted into the bit line; An annealing process is used to diffuse the doping material from the bit line into the drain region of the silicon semiconductor column.

15. The method for manufacturing a semiconductor device according to any one of claims 10 to 14, wherein: The silicon semiconductor column further comprises a source region, and the source region is located on a side of the channel region away from the silicon substrate; The method for manufacturing the semiconductor device further comprises: performing low-energy ion implantation in the source region by using a self-aligned ion implantation process, and annealing and diffusion to form a doping region containing doping materials in the source region.

16. The method for manufacturing a semiconductor device according to claim 15, wherein: The source region and the drain region are doped simultaneously through a self-aligned ion implantation process, and the doped region of the source region and the doped region of the drain region are formed simultaneously through an annealing process.

17. The method for manufacturing a semiconductor device according to claim 15, wherein: The implantation depth of the doping material in the silicon substrate and / or the source region is 0 to 45 nm.

18. The method for manufacturing a semiconductor device according to any one of claims 10 to 17, wherein: The process conditions of the low-energy ion implantation in the drain region and / or the source region include: an implantation energy of 5kev to 100kev.

19. The method for manufacturing a semiconductor device according to any one of claims 10 to 17, wherein: The annealing process conditions include: an annealing temperature of 850° C. to 1100° C., and an annealing time of 5 seconds to 30 seconds.

20. An electronic device comprising the semiconductor device according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Memory and manufacturing method thereof

    CN113594163A

  • Semiconductor structure and manufacturing method thereof

    CN114759030A

  • Semiconductor device and preparation method thereof, and electronic equipment

    CN115832015A