Lithium supplementing composite separator for lithium battery, lithium battery, and preparation method therefor

By using a lithium-replenishing composite separator in a lithium battery, including a separator layer, a metallic lithium layer, an electronic conductive layer and a protective layer, the problems of low first Coulombic efficiency and poor cycle life of lithium batteries are solved, and the performance and safety of lithium batteries are improved. , simplifying the production process and reducing storage environment requirements.

WO2024198536A1PCT designated stage expired Publication Date: 2024-10-03ADVANCED MATERIALS TECH (BEIJING) CO LTD

Patent Information

Application Number
PCT/CN2023/139267
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2023-12-15
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing lithium batteries have low initial Coulombic efficiency and poor cycle life, mainly due to the unstable electrode interface caused by the volume change of the negative electrode material during the charge and discharge process. The existing pre-lithiation method is complex to operate, costly and has high environmental requirements, which affects production. Efficiency and safety.

Method used

A lithium-replenishing composite separator is used, including a separator layer, a metallic lithium layer, an electronic conductive layer and a protective layer. The separator layer is isolated from the positive electrode layer, the metallic lithium layer is connected to the negative electrode layer, the electronic conductive layer provides a conductive channel, and the protective layer prevents lithium The layer reacts with the environment to ensure the stability and safety of lithium batteries.

Benefits of technology

Improves the first Coulombic efficiency and cycle life of lithium batteries, reduces pre-lithium costs, reduces lithium losses, simplifies the production process, reduces storage environment requirements, and enhances the performance of lithium batteries by forming solid electrolyte films in situ .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023139267_03102024_PF_FP_ABST
    Figure CN2023139267_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application provides a lithium supplementing composite separator for a lithium battery, a lithium battery, and a preparation method therefor. The lithium battery comprises a negative electrode layer and a positive electrode layer, and the lithium supplementing composite separator is provided between the negative electrode layer and the positive electrode layer. The lithium supplementing composite separator comprises: a separator layer, configured to isolate the negative electrode layer from the positive electrode layer; a lithium metal layer, provided on the side of the separator layer close to the negative electrode layer, and configured to supplement lithium to the negative electrode layer; a first protective layer, provided on the side of the lithium metal layer close to the negative electrode layer; and an electron-conductive layer, provided on the side of the lithium metal layer close to the negative electrode layer, and configured to provide an electron-conductive channel between the lithium metal layer and the negative electrode layer, wherein the orthographic projections of the electron-conductive layer and the first protective layer on the lithium metal layer do not overlap or partially overlap.
Need to check novelty before this filing date? Find Prior Art

Description

A lithium-supplementing composite diaphragm for lithium batteries, lithium batteries and preparation methods thereof

[0001] This application claims priority to Chinese patent application No. 202310323013.1, filed on March 29, 2023. This application incorporates the entire text of the aforementioned Chinese patent application. Technical Field

[0002] The present application relates to the technical field of lithium batteries, and in particular to a lithium-supplementing composite diaphragm for lithium batteries, a lithium battery, and a preparation method thereof. Background Art

[0003] Lithium-ion batteries, as highly efficient energy storage devices, are widely used in daily life. However, with the rapid development of technologies such as electronic products and electric vehicles, the demand for lithium-ion batteries' energy density and cycle life has continued to increase, leading to the increasing use of anode materials with high theoretical specific capacities, such as Si-based, Si-O-based, and alloys. However, these anode materials experience significant volume changes during the charge and discharge process, resulting in an unstable electrode interface. This leads to low initial coulombic efficiency and poor cycling performance.

[0004] In order to solve the above problems, people have adopted many methods, such as chemical reduction method, artificial SEI film method, negative electrode pre-lithiation method, etc. Among them, negative electrode pre-lithiation method is the most direct solution.

[0005] Currently, methods for negative electrode pre-lithiation are primarily categorized into four types: 1. Electrochemical pre-lithiation; 2. Chemical pre-lithiation; 3. Lithium metal patch method (contact method); and 4. Stable lithium metal powder method. However, all four methods present various challenges. The electrochemical pre-lithiation method is complex to operate and consumes a lot of energy, resulting in high pre-lithiation costs. The chemical pre-lithiation method is highly hazardous because the lithium source used is generally unstable, flammable, and explosive. The stable lithium metal powder method is also highly hazardous, and its raw materials are expensive, resulting in high pre-lithiation costs. While the lithium metal patch method (contact method) is more convenient to operate, its lithium metal utilization rate is very low, resulting in high pre-lithiation costs. Furthermore, the use of lithium metal also makes it highly hazardous. Furthermore, the lithium metal patch method places high demands on the humidity of the electrode pre-lithiation environment and the storage and use environment after pre-lithiation, further increasing the pre-lithiation cost. Furthermore, all four pre-lithiation methods require new processes, altering the existing lithium battery manufacturing process, and reducing lithium battery production efficiency.

[0006] Therefore, there is an urgent need for an efficient and convenient pre-lithiation method that can stably pre-lithiate the negative electrode of the lithium battery without reducing the production efficiency of the lithium battery and having no excessively high requirements on the production and storage environment.

[0007] Summary of the Invention

[0008] The purpose of the present application is to provide a lithium-supplementing composite diaphragm for lithium batteries, a lithium battery and a preparation method thereof, which can solve the technical problem of low initial coulombic efficiency of current lithium batteries.

[0009] The present invention provides a lithium-supplementing composite diaphragm for a lithium battery. The lithium battery includes a negative electrode layer and a positive electrode layer. The lithium-supplementing composite diaphragm is disposed between the negative electrode layer and the positive electrode layer. The lithium-supplementing composite diaphragm includes:

[0010] a separator layer configured to separate the negative electrode layer from the positive electrode layer;

[0011] a metallic lithium layer, disposed on a side of the separator layer close to the negative electrode layer, and configured to supplement lithium to the negative electrode layer;

[0012] A first protective layer is provided on a side of the metal lithium layer close to the negative electrode layer;

[0013] an electronic conductive layer, disposed on a side of the metallic lithium layer close to the negative electrode layer, and configured to provide an electronic conductive path between the metallic lithium layer and the negative electrode layer;

[0014] The orthographic projections of the electronic conductive layer and the first protective layer on the metallic lithium layer do not overlap or partially overlap.

[0015] In some embodiments, the lithium-supplementing composite diaphragm further comprises:

[0016] The second protective layer is arranged on a side of the metal lithium layer away from the negative electrode layer.

[0017] In some embodiments, the lithium-supplementing composite diaphragm further comprises:

[0018] The second protective layer is arranged on a side of the diaphragm layer away from the metal lithium layer.

[0019] In some embodiments, the orthographic projection shape of the electronic conductive layer on the metallic lithium layer is an island shape, wherein the island shape includes a plurality of discontinuous island shapes and / or at least one network shape formed by connecting a plurality of island shapes.

[0020] In some embodiments, the thickness of the electronically conductive layer is greater than the thickness of the first protective layer.

[0021] In some embodiments, the thickness of the electronically conductive layer is 10 nm to 1000 nm.

[0022] In some embodiments, the coverage of the electronic conductive layer on the metallic lithium layer is 10%-90%.

[0023] In some embodiments, the area of ​​a single electronic conductive layer is 100 nm 2 ~1000000nm 2 .

[0024] In some embodiments, the thickness of the first protective layer and / or the second protective layer is 10 nm-1000 nm.

[0025] In some embodiments, the thickness of the metal lithium layer is 0.1 μm-10 μm, and the metal lithium layer has a dense or porous structure.

[0026] In some embodiments, the material of the electronic conductive layer includes at least one of the following: metal, metal oxide, metal nitride, metal sulfide or carbon material.

[0027] In some embodiments, the metal material includes at least one of the following: gold, silver, copper, iron, titanium, aluminum, manganese, tin, cobalt, nickel, chromium, bismuth, vanadium, molybdenum, or niobium;

[0028] The carbon material includes at least one of the following: graphite, hard carbon, soft carbon, graphene or carbon nanotube.

[0029] In some embodiments, the material of the first protective layer and / or the second protective layer includes at least one of the following:

[0030] Al2O3, MgO, ZnO2, TiO2, ZrO2, LaO2, CeO2, Y2O3, Si x O, SiC, SiN x 、SiCN x , AlN, Mg(OH)2, BaSO4, boehmite or perovskite; or,

[0031] Li2CO3, Li3N, LiF, Li3PO4, Li4SiO4, Li4Ti5O 12 , LiPON, LiSiON, LLZO, LLZTO, LATP, Li3Fe2(PO4)3, Li3V2(PO4)3, Li3In2(PO4)3, Li3Sc2(PO4)3, Li3Cr2(PO4)3.

[0032] In some embodiments, the diaphragm layer is one of the following: a basement membrane, a basement membrane / ceramic composite diaphragm, a basement membrane / adhesive composite diaphragm, or a basement membrane / ceramic / adhesive composite diaphragm.

[0033] In some embodiments, the base film comprises at least one of the following: a polyethylene base film, a polyethylene non-woven base film, a polypropylene base film, a polypropylene non-woven base film, a polypropylene / polyethylene / polypropylene composite base film, a polyimide base film, a polyimide non-woven base film, a polytetrafluoroethylene base film, a polytetrafluoroethylene non-woven base film, a polyvinyl chloride base film or a polyvinyl chloride non-woven base film; and / or,

[0034] The ceramic comprises at least one of the following: alumina, zirconia, boehmite, magnesium hydroxide, barium sulfate, silicon oxide, aluminum nitride, magnesium oxide, titanium dioxide, yttrium oxide or cerium oxide; and / or,

[0035] The adhesive comprises at least one of the following: polytetrafluoroethylene, polyvinylidene fluoride, acrylic acid, polyethylene oxide, sodium carboxymethyl cellulose, styrene-butadiene rubber, hydroxypropyl methylcellulose, carboxystyrene-butadiene latex or polyvinyl alcohol.

[0036] In some embodiments, the lithium layer includes at least one of metallic lithium, lithium silicon alloy, lithium magnesium alloy, lithium copper alloy, lithium silver alloy, lithium beryllium alloy, lithium zinc alloy, lithium cadmium alloy, lithium aluminum alloy, lithium gold alloy, and lithium boron alloy.

[0037] An embodiment of the present application provides a lithium battery, comprising a lithium-supplementing composite separator as described above, wherein the negative electrode layer comprises a negative electrode current collector layer and a negative electrode active material layer covering the negative electrode current collector layer; and the positive electrode layer comprises a positive electrode current collector layer and a positive electrode active material layer covering the positive electrode current collector layer.

[0038] The present invention provides a method for preparing a lithium-supplementing composite diaphragm, comprising the following steps:

[0039] providing a diaphragm layer;

[0040] forming a metallic lithium layer on one side of the separator layer;

[0041] forming an electronic conductive layer on the surface of the metallic lithium layer;

[0042] A first protective layer is formed on the surface of the metallic lithium layer, wherein the orthographic projections of the electronic conductive layer and the first protective layer on the metallic lithium layer do not overlap or partially overlap.

[0043] In some embodiments, forming a metallic lithium layer on one side of the separator layer comprises:

[0044] forming a second protective layer on one side of the diaphragm layer;

[0045] A metal lithium layer is formed on the surface of the second protective layer.

[0046] In some embodiments, forming a metallic lithium layer on one side of the separator layer comprises:

[0047] forming a second protective layer on one side of the diaphragm layer;

[0048] A metallic lithium layer is formed on a side of the separator layer opposite to the second protective layer.

[0049] In some embodiments, the method for forming the first protective layer and / or the second protective layer includes at least one of the following:

[0050] Doctor coating, roller coating, spray coating, chemical vapor deposition, plasma vapor deposition, atomic layer deposition, pulsed laser deposition, vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering.

[0051] In some embodiments, the method for forming the electronic conductive layer includes at least one of the following: blade coating, roller coating, spray coating, chemical vapor deposition, plasma vapor deposition, atomic layer deposition, pulsed laser deposition, vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering.

[0052] In some embodiments, the method for forming the metallic lithium layer comprises at least one of the following:

[0053] Vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering.

[0054] The present invention provides a method for preparing a lithium battery, comprising the following steps:

[0055] Prepare a lithium battery negative electrode, wherein the lithium battery negative electrode comprises a negative electrode current collector layer and a negative electrode active material layer covering the negative electrode current collector layer;

[0056] Prepare a lithium battery positive electrode, wherein the lithium battery positive electrode comprises a positive electrode current collector layer and a positive electrode active material layer covering the positive electrode current collector layer;

[0057] Prepare a lithium-supplementing composite diaphragm, wherein the preparation method of the lithium-supplementing composite diaphragm adopts any of the methods described above;

[0058] The lithium-supplementing composite separator is assembled between the negative electrode and the positive electrode of the lithium battery, so that the electronic conductive layer is attached to the negative electrode active material layer.

[0059] Compared with the prior art, the embodiments of the present application have the following technical effects:

[0060] The lithium-replenishing composite separator described herein can be directly used to replenish lithium in negative electrodes. It provides both electronic and ionic conductive pathways between the lithium layer and the negative electrode active material. After battery assembly, it forms an in-situ solid electrolyte interlayer (SEI), reducing active lithium loss and improving the coulombic efficiency and cycle life of the lithium battery. Furthermore, the lithium-replenishing composite separator described herein, with protective layers on both sides of the lithium layer, isolates the lithium layer from the external environment, preventing it from reacting with air and / or water in the environment. This results in relatively low storage requirements for the separator. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] The accompanying drawings are incorporated into and constitute a part of the specification, illustrating embodiments consistent with the present application and, together with the specification, explaining the principles of the present application. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can derive other drawings based on these drawings without inventive effort. In the drawings:

[0062] FIG1 is a schematic structural diagram of a lithium-supplementing composite diaphragm according to some embodiments of the present application.

[0063] FIG2 is a schematic diagram of the pattern structure of the electronic conductive layer of the lithium-supplementing composite separator according to some embodiments of the present application.

[0064] FIG3 is a schematic structural diagram of lithium-supplementing composite diaphragms according to some other embodiments of the present application.

[0065] FIG4 is a schematic structural diagram of lithium-supplementing composite diaphragms according to some other embodiments of the present application.

[0066] FIG5 is a schematic structural diagram of lithium-supplementing composite diaphragms according to some other embodiments of the present application.

[0067] FIG6 is a schematic structural diagram of a lithium battery according to some embodiments of the present application.

[0068] FIG7 is a schematic structural diagram of lithium batteries according to some other embodiments of the present application.

[0069] FIG8 is a flow chart of a method for preparing a lithium-supplementing composite diaphragm according to some embodiments of the present application.

[0070] FIG9 is a flow chart of a lithium battery preparation method according to some embodiments of the present application.

[0071] FIG10 is a schematic diagram of open circuit voltage variation curves of some embodiments and comparative examples of the present application.

[0072] FIG11 is a schematic diagram of the first charge and discharge curves of some embodiments and comparative examples of the present application.

[0073] FIG12 is a schematic diagram of the experimental results of the initial states of Example 1 and Example 2 of the present application.

[0074] FIG13 is a schematic diagram of the experimental results of Example 1 and Example 2 of the present application after being placed for 15 days.

[0075] FIG14 is a schematic diagram of the experimental results of Example 1 and Example 2 of the present application after being placed for 30 days.

[0076] FIG15 is a schematic diagram of the open circuit voltage change curves of some embodiments and comparative examples of the present application after 30 days of storage.

[0077] FIG16 is a schematic diagram of normal temperature cycle results of some embodiments and comparative examples of the present application. DETAILED DESCRIPTION

[0078] To make the objectives, technical solutions, and advantages of this application more clear, this application will be further described in detail below with reference to the accompanying drawings. Obviously, the embodiments described are only some of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of this application.

[0079] The terms used in the examples of this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The singular forms "a," "the," and "the" used in the examples of this application and the appended claims are also intended to include plural forms, and unless the context clearly indicates otherwise, "a plurality" generally includes at least two.

[0080] It should be understood that the term "and / or" as used herein is merely a description of the relationship between associated objects, indicating that three possible relationships exist. For example, "A and / or B" can represent: A exists alone, A and B exist simultaneously, or B exists alone. Furthermore, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.

[0081] It should be understood that although the terms first, second, third, etc. may be used to describe in the embodiments of the present application, these should not be limited to these terms. These terms are only used to distinguish. For example, without departing from the scope of the embodiments of the present application, the first may also be referred to as the second, and similarly, the second may also be referred to as the first.

[0082] It should also be noted that the terms "include," "comprises," or any other variations thereof are intended to encompass non-exclusive inclusion, such that a product or device comprising a series of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such product or device. In the absence of further limitations, an element defined by the phrase "comprising a" does not exclude the presence of other identical elements in the product or device comprising the element.

[0083] In the relevant technologies for the preparation of lithium batteries, due to the poor electronic conductivity and lithium ion conductivity of the positive and negative electrode separators used in lithium-ion batteries, the lithium-ion batteries have low initial coulombic efficiency (Coulombic efficiency refers to the ratio of the battery's discharge capacity to the charging capacity during the same cycle, because the input electricity is often not all used to convert the active material into a charged state, but some is consumed, such as irreversible side reactions, so the coulombic efficiency is often less than 100%), as well as poor cycle performance and other shortcomings. Pre-lithiation or lithium replenishment of the negative electrode is the most direct method to improve the performance of the negative electrode. Therefore, there is an urgent need for an efficient and convenient lithium replenishment method that can stably replenish lithium to the negative electrode of the lithium battery without reducing the production efficiency of the lithium battery and without excessively high requirements for the production and storage environment.

[0084] An embodiment of the present application provides a lithium-replenishing composite diaphragm for a lithium battery, wherein the lithium battery includes a negative electrode layer and a positive electrode layer, and the lithium-replenishing composite diaphragm is arranged between the negative electrode layer and the positive electrode layer to isolate the negative electrode layer and the positive electrode layer, while replenishing lithium to the negative electrode layer, wherein the lithium-replenishing composite diaphragm includes: a diaphragm layer, configured to isolate the negative electrode layer and the positive electrode layer; a metallic lithium layer, arranged on a side of the diaphragm layer close to the negative electrode layer, configured to replenish lithium to the negative electrode layer; a first protective layer, arranged on a side of the metallic lithium layer close to the negative electrode layer; an electronic conductive layer, arranged on a side of the metallic lithium layer close to the negative electrode layer, configured to provide an electronic conductive channel between the metallic lithium layer and the negative electrode layer; wherein the electronic conductive layer and the first protective layer do not overlap or partially overlap on the orthographic projection of the metallic lithium layer.

[0085] The lithium-replenishing composite diaphragm of the present application can be directly applied to the negative electrode lithium replenishment, thereby improving the initial coulombic efficiency and cycle life of the lithium battery. The lithium-replenishing composite diaphragm of the present application can control the degree of lithium replenishment (pre-lithiation) by regulating the thickness of the metal lithium layer, and improves the utilization rate of lithium in the pre-lithiation process. The composite diaphragm of the present application provides an electronic conductive channel between the metal lithium layer and the negative electrode active material, thereby reducing the generation of dead lithium and further improving the utilization rate of lithium. The lithium-replenishing composite diaphragm of the present application does not change the normal production process flow of the lithium battery and will not reduce the production efficiency of the lithium battery. The lithium-replenishing composite diaphragm of the present application has a protective layer on both sides of the metal lithium layer, which isolates the metal lithium layer from the external environment, so that the metal lithium layer does not react with the air and / or water in the environment, so the lithium-replenishing composite diaphragm has relatively low requirements for the storage environment. In addition, the lithium-supplementing composite diaphragm of the present application provides an electronic conductive path and an ion conductive path between the metallic lithium layer and the negative electrode active material. After the battery is assembled, a solid electrolyte film (SEI) can be formed in situ, further reducing the loss of active lithium and improving the coulombic efficiency and cycle life of the lithium battery.

[0086] The optional embodiments of the present application are described in detail below with reference to the accompanying drawings.

[0087] As shown in Figures 1 and 6, an embodiment of the present application provides a lithium-replenishing composite diaphragm 1 for a lithium battery. The lithium battery includes a negative electrode layer 3 and a positive electrode layer 4. The lithium-replenishing composite diaphragm 1 is arranged between the negative electrode layer 3 and the positive electrode layer 4. The lithium-replenishing composite diaphragm 1 can directly replenish lithium to the negative electrode layer 3 of the lithium battery, thereby improving the initial coulombic efficiency and cycle life of the lithium battery. As shown in Figure 6, the negative electrode layer 3 includes a negative electrode current collector layer 301 and a negative electrode active material layer 302, and the positive electrode layer 4 includes a positive electrode current collector layer 401 and a positive electrode active material layer 402. As shown in Figure 1, the lithium-replenishing composite diaphragm 1 includes: a diaphragm layer 101, configured to separate the negative electrode layer 3 and the positive electrode layer 4; a metallic lithium layer 103, arranged on the side of the diaphragm layer 101 close to the negative electrode layer 3, configured to replenish lithium to the negative electrode layer 3; a first protective layer 105, arranged on the side of the metallic lithium layer 103 close to the negative electrode layer 3; an electronic conductive layer 104, arranged on the side of the metallic lithium layer 103 close to the negative electrode layer 3, configured to provide an electronic conductive channel between the metallic lithium layer 103 and the negative electrode layer 3; wherein the electronic conductive layer 104 and the first protective layer 105 do not overlap or partially overlap on the orthographic projection of the metallic lithium layer 103.

[0088] In some embodiments, as shown in FIG1 and FIG6 , the separator layer 101 is used to separate the negative electrode layer 3 and the positive electrode layer 4, and its thickness is generally 5 μm-300 μm, for example, 50 μm, 100 μm, 200 μm, 250 μm, etc., which will not be described in detail here. Different thicknesses can be selected according to the type of material of the separator layer 101. If the thickness of the separator layer 101 is greater than 300 μm, the preparation efficiency of the lithium battery will be reduced. If the thickness of the separator layer 101 is less than 5 μm, the positive and negative electrodes of the lithium battery will be easily broken down, resulting in a short circuit.

[0089] In some embodiments, the types of diaphragm layers may include base membrane, base membrane / ceramic composite diaphragm, base membrane / adhesive composite diaphragm, and base membrane / ceramic / adhesive composite diaphragm.

[0090] Among them, the base film can be at least one of a polyethylene base film, a polyethylene non-woven base film, a polypropylene base film, a polypropylene non-woven base film, a polypropylene / polyethylene / polypropylene composite base film, a polyimide base film, a polyimide non-woven base film, a polytetrafluoroethylene based film, a polytetrafluoroethylene non-woven base film, a polyvinyl chloride based film, and a polyvinyl chloride non-woven base film, or a combination of several of them, and there is no limitation on the type and quantity of the combination.

[0091] The ceramic may be at least one or a combination of alumina, zirconia, boehmite, magnesium hydroxide, barium sulfate, silicon oxide, aluminum nitride, magnesium oxide, titanium dioxide, yttrium oxide, and cerium oxide, and the type and quantity of the combination are not limited.

[0092] The adhesive can be at least one of polytetrafluoroethylene, polyvinylidene fluoride, acrylic acid, polyethylene oxide, carboxymethyl cellulose sodium, styrene-butadiene rubber, hydroxypropyl methylcellulose, carboxystyrene-butadiene latex, and polyvinyl alcohol, or a combination thereof, and the type and quantity of the combination are not limited.

[0093] In some embodiments, as shown in Figures 1 and 6, the metal lithium layer 103 serves as a core layer for replenishing lithium and is disposed on one side of the diaphragm layer 101 close to the negative electrode layer 3. The thickness of the metal lithium layer is 0.1 μm-10 μm, for example, 0.1 μm-0.3 μm, 0.3 μm-1 μm, 1 μm-3 μm, 3 μm-6 μm, 6 μm-10 μm, etc., which will not be described in detail here. Different thicknesses can be selected according to the type of material of the metal lithium layer. The degree of lithium replenishment (pre-lithiation) can be controlled by regulating the thickness of the metal lithium layer, and the utilization rate of lithium in the pre-lithiation process can be improved. Among them, the surface of the metal lithium layer can be made of a dense material or a porous loose structure material, which is not limited to this.

[0094] In some embodiments, the material of the metallic lithium layer can be pure metallic lithium, a lithium alloy material, or a composite layer of pure metallic lithium and lithium alloy materials, wherein the lithium alloy material, for example, includes at least one or a combination of the following: metallic lithium, lithium silicon alloy, lithium magnesium alloy, lithium copper alloy, lithium silver alloy, lithium beryllium alloy, lithium zinc alloy, lithium cadmium alloy, lithium aluminum alloy, lithium gold alloy and lithium boron alloy. The free combination of the above-mentioned multiple materials is not specifically limited.

[0095] In some embodiments, as shown in Figures 1 and 6, a first protective layer 105 is disposed on a side of the metallic lithium layer 103 close to the negative electrode layer 3. The first protective layer 105 is a layer disposed between the metallic lithium layer 103 and the negative electrode layer 3. The first protective layer 105 partially covers the metallic lithium layer 103, for example, partially covers 10%-90% of the metallic lithium layer 103 to prevent the metallic lithium layer 103 from being partially or completely exposed to air, water-containing air and / or water. Since the metallic lithium layer is easy to react with air or water, the first protective layer 105 isolates the metallic lithium layer from the external environment, isolates the metallic lithium layer from contact with air and / or moisture, reduces the occurrence of side reactions of the metallic lithium layer, and protects the metallic lithium layer, thereby reducing its requirements for the storage environment.

[0096] In some embodiments, the thickness of the first protective layer is 10nm-1000nm, for example, 10nm-100nm, 100nm-300nm, 300nm-600nm, 600nm-900nm, 1000nm, etc., which are not described here. Different thicknesses can be selected according to the material type of the first protective layer.

[0097] In some embodiments, the first protective layer is made of a material with high ionic conductivity. While providing protection for the metallic lithium layer, it can also improve the ionic conductivity of the entire lithium-replenishing composite diaphragm, thereby improving the efficiency and effectiveness of lithium replenishment during its use. Specifically, the first protective layer material can be selected from at least one of the following or a combination of several, with no limitation on the type and quantity of the combination:

[0098] Al2O3, MgO, ZnO2, TiO2, ZrO2, LaO2, CeO2, Y2O3, Si x O, SiC, SiN x 、SiCN x , AlN, Mg(OH)2, BaSO4, boehmite or perovskite; or,

[0099] Li2CO3, Li3N, LiF, Li3PO4, Li4SiO4, Li4Ti5O 12, lithium phosphorus oxynitride (LiPON), LiSiON, lithium lanthanum zirconium oxide (LLZO), tantalum-doped lithium lanthanum zirconium oxide (LLZTO), lithium aluminum titanium phosphate (LATP), Li3Fe2(PO4)3, Li3V2(PO4)3, Li3In2(PO4)3, Li3Sc2(PO4)3, Li3Cr2(PO4)3.

[0100] In some embodiments, as shown in Figures 1 and 6, the electronic conductive layer 104 is arranged on the side of the metal lithium layer 103 close to the negative electrode layer 3, and is configured to provide an electronic conductive channel between the metal lithium layer 103 and the negative electrode layer 3; the electronic conductive layer 104 and the first protective layer 105 are both arranged on the surface of the metal lithium layer 103, and the electronic conductive layer 104 and the first protective layer 105 do not overlap or partially overlap in the orthographic projection of the metal lithium layer 103. For example, the electronic conductive layer in Figure 1 is in the shape of a column 1043, which does not overlap with the positive projection of the first protective layer 105 on the metallic lithium layer 103; for example, the electronic conductive layer in Figure 1 is in the shape of an inverted cone or an inverted table 1042, or the electronic conductive layer is in the shape of a right cone or a right table 1041. The cone or table shape can be a regular cone or table shape, such as a cone or a truncated cone shape, or an irregular cone or table shape, which partially overlaps with the positive projection of the first protective layer 105 on the metallic lithium layer 103, that is, there is overlap at the edge, and the overlapping range is small, which does not affect the electronic conductive layer from providing an electronic conductive channel. The arrangement in which the electronic conductive layer 104 and the first protective layer 105 partially overlap on the orthographic projection of the metallic lithium layer 103 can increase the sealing performance between the electronic conductive layer 104 and the first protective layer 105, so that there is no gap between the electronic conductive layer 104 and the first protective layer 105, thereby ensuring that the electronic conductive layer 104 and the first protective layer 105 can completely cover the metallic lithium layer 103 100%, further completely isolating the metallic lithium layer from the external environment, isolating the metallic lithium layer from contact with air and / or moisture, reducing the possibility of side reactions in the metallic lithium layer, and providing absolute protection for the metallic lithium layer.

[0101] As an example to illustrate the advantages of the cone-shaped or terrace-shaped electronic conductive layer, for example, one method of forming the electronic conductive layer 104 and the first protective layer 105 is to set a mask for the electronic conductive layer, first form the first protective layer by one or a combination of any two or more methods such as scraping, roller coating, spraying, chemical vapor deposition, plasma vapor deposition, atomic layer deposition, pulsed laser deposition, etc., then remove the mask, and then form the electronic conductive layer 104 by one or a combination of any two or more sputtering methods such as RF sputtering, magnetron sputtering or reactive sputtering. At this time, each conductive unit in the electronic conductive layer is formed into a cone or terrace shape, which can significantly reduce the gap between each conductive unit and the protective layer, thereby improving the protection of the metallic lithium layer.

[0102] As a specific embodiment, the orthographic projections of the electronic conductive layer 104 and the first protective layer 105 on the metallic lithium layer 103 do not overlap, and both are regular columnar shapes 1043. A regular matrix-arranged electronic conductive layer 104 can be formed through a mask process to enhance the uniformity of the electronic conductive layer 104.

[0103] As a specific embodiment, the electronic conductive layer 104 and the first protective layer 105 overlap on the positive projection of the metal lithium layer 103, and both are irregular inverted cone or inverted table shape 1042 or regular cone or regular table shape 1041. A matrix-arranged electronic conductive layer 104 can be formed by a sputtering process to enhance the sealing of the electronic conductive layer 104.

[0104] In some embodiments, as shown in Figure 2, the orthographic projection shape of the electronic conductive layer 104 on the metallic lithium layer 103 is an island shape, and the island shape means that the orthographic projection of the electronic conductive layer 104 on the metallic lithium layer 103 is an isolated discontinuous conductive unit, wherein the island shape includes one or more discontinuous conductive units 1044 and / or at least one network 1045 formed by connecting multiple conductive units. The electronic conductive layer 104 is arranged on the metallic lithium layer 103 in a regular or irregular pattern. For example, the positive projection of the electronic conductive layer 104 on the metallic lithium layer 103 can be a discontinuous island pattern 1044 or a mesh pattern 1045. The discontinuous island pattern 1044 can be a cluster of multiple island patterns gathered together but not connected. The mesh pattern 1045 can be a continuous island pattern composed of multiple island patterns next to each other, that is, multiple conductive units are interconnected. There is no limitation on this. The mesh pattern 1045 can be a linear connection of multiple island units through conductive material, maintaining the electrical conductivity of multiple island units without changing the position occupied by a single island structure. When one of the island-shaped conductive units becomes non-conductive, electrons can still be transmitted through other island-shaped conductive units, without changing the conductive area and thus not significantly reducing the conductivity of the electronic conductive layer 104. For the electronic conductive layer 104, the process required to form one or more discontinuous conductive units 1044 and / or at least one network 1045 formed by connecting multiple conductive units is simple. During the sputtering process, there is no need to specifically control the position of the sputtering point or the amount of sputtered material to form island-shaped conductive units. During the process of forming the first protective layer through the evaporation process, the growth position of the evaporated material can be flexibly controlled. After the conical conductive units are sputtered, a dense protective layer can be formed around the island-shaped conductive units through the evaporation process, thereby enhancing the isolation protection of the metal lithium layer. In some embodiments, the thickness of the electronic conductive layer 104 is greater than the thickness of the first protective layer 105, so as to prioritize ensuring that the metal lithium layer 103 and the negative electrode layer 3 are fully connected through the electronic conductive layer 104, providing an electronic conductive channel for the metal lithium layer 103 to the negative electrode layer 3, thereby improving the lithium replenishment efficiency. The electronic conductive layer provides a high-speed electron conduction channel between the metallic lithium layer and the negative electrode active material, increasing the reaction sites between the metallic lithium layer and the negative electrode active material, improving the reaction rate of the metallic lithium layer, and improving the efficiency of lithium replenishment. It can also reduce or even avoid the generation of dead lithium, improve the utilization rate of the metallic lithium layer, and reduce costs. Without the electronic conductive layer, metallic lithium is prone to agglomeration, resulting in a large amount of dead lithium. After adding the electronic conductive layer, the reaction sites between the lithium layer and the negative electrode active material increase, the current density is dispersed, and agglomeration is less likely to occur. This can effectively reduce the generation of dead lithium, improve the utilization rate of the lithium layer, and thus save costs.

[0105] In some embodiments, the thickness of the electronic conductive layer is 10nm-1000nm, for example, 10nm-100nm, 100nm-300nm, 300nm-600nm, 600nm-900nm, 1000nm, etc., which are not described here. Different thicknesses can be selected according to the material type of the electronic conductive layer.

[0106] In some embodiments, as shown in Figures 1 and 2, the coverage of the metal lithium layer 103 by the electronic conductive layer 104 is 10%-90%, and together with the first protective layer 105, it completes 100% coverage of the metal lithium layer 103, making it completely impossible for the surface of the metal lithium layer 103 to be exposed to air, water-containing air and / or water, completely isolating the lithium layer from contact with air and / or moisture, reducing the occurrence of side reactions in the lithium layer, and also protecting the metal lithium layer, reducing its requirements for the storage environment.

[0107] In some embodiments, when the electronic conductive layer is distributed in multiple discontinuous islands, the area of ​​a single conductive unit can be 100 nm. 2 ~1000000nm 2 , for example, you can choose 100nm 2 ~100000nm 2 , 100000nm 2 ~500000nm 2 , 500000nm 2 ~1000000nm 2 Etc., which will not be elaborated here. Different areas can be selected according to the material type of the electronic conductive layer to ensure that the metal lithium layer and the negative electrode layer are fully conductive.

[0108] In some embodiments, the material of the electronically conductive layer includes at least one of the following, or a random combination of several: metal, metal oxide, metal nitride, metal sulfide, or carbon material. The metal material includes at least one of the following: gold, silver, copper, iron, titanium, aluminum, manganese, tin, cobalt, nickel, chromium, bismuth, vanadium, molybdenum, or niobium; the metal oxide, metal nitride, or metal sulfide is a metal oxide, metal nitride, or metal sulfide of gold, silver, copper, iron, titanium, aluminum, manganese, tin, cobalt, nickel, chromium, bismuth, vanadium, molybdenum, or niobium. The carbon material includes at least one of the following: graphite, hard carbon, soft carbon, graphene, or carbon nanotubes.

[0109] The lithium-supplementing composite diaphragm of the present application provides an electronic conductive path and an ion conductive path between the metallic lithium layer and the negative electrode active material. After the battery is assembled, a solid electrolyte film (SEI) can be formed in situ, further reducing the loss of active lithium and improving the coulombic efficiency and cycle life of the lithium battery.

[0110] In some embodiments, as shown in FIG3 , based on the above-described embodiment, the lithium-supplementing composite separator 1 further includes a second protective layer 102 , which is disposed on a side of the lithium metal layer 103 away from the negative electrode layer 3 , as understood in conjunction with FIG6 . In this embodiment, the second protective layer 102 is attached to the side of the lithium metal layer 103 opposite to the first protective layer 105 . By disposing the first protective layer 105 and the second protective layer 102 on the upper and lower surfaces of the lithium metal layer 103 , respectively, the risk of exposure of the other side of the lithium metal layer 103 can be further isolated, thereby preventing the lithium metal layer 103 from being partially or completely exposed to air, water-containing air, and / or water. Partial exposure can be caused by the permeation of other non-compact membrane layers (e.g., air-permeable or water-permeable), which may cause the lithium metal layer 103 to react with air or water. Therefore, by disposing the second protective layer 102 , the lithium metal layer can be further completely isolated from the external environment, isolating the lithium metal layer from contact with air and / or water, further reducing the occurrence of side reactions of the lithium metal layer, and further protecting the lithium metal layer, thereby reducing its requirements for the storage environment.

[0111] In some embodiments, the thickness of the second protective layer is 10nm-1000nm, for example, 10nm-100nm, 100nm-300nm, 300nm-600nm, 600nm-1000nm, etc., which are not described here. Different thicknesses can be selected according to the material type of the second protective layer.

[0112] In some embodiments, the second protective layer is made of a material with high ionic conductivity. While providing protection for the metallic lithium layer, it can also improve the ionic conductivity of the entire lithium-replenishing composite diaphragm, thereby improving the efficiency and effectiveness of lithium replenishment during its use. Specifically, the material of the second protective layer can be selected from at least one of the following or a combination thereof, without limitation:

[0113] Al2O3, MgO, ZnO2, TiO2, ZrO2, LaO2, CeO2, Y2O3, Si x O, SiC, SiN x 、SiCN x , AlN, Mg(OH)2, BaSO4, boehmite or perovskite; or,

[0114] Li2CO3, Li3N, LiF, Li3PO4, Li4SiO4, Li4Ti5O 12 , LiPON, LiSiON, LLZO, LLZTO, LATP, Li3Fe2(PO4)3, Li3V2(PO4)3, Li3In2(PO4)3, Li3Sc2(PO4)3, Li3Cr2(PO4)3.

[0115] In some other embodiments, as shown in FIG4 , based on the above embodiment, the lithium-supplementing composite separator 1 further includes a second protective layer 102 , which is disposed on a side of the separator layer 101 away from the metallic lithium layer 103 . In this embodiment, the second protective layer 102 is attached to the side of the diaphragm layer 101 opposite to the first protective layer 105. By arranging the second protective layer 102 on the lower surface of the diaphragm layer 101, the upper and lower surfaces of the metal lithium layer 103 are indirectly provided with the first protective layer 105 and the second protective layer 102, respectively, which can further isolate the exposure risk of the other side of the metal lithium layer 103 to avoid partial or complete exposure of the metal lithium layer 103 to air, water-containing air and / or water. By arranging the second protective layer 102 on the lower surface of the diaphragm layer 101, the first protective layer 105 and the second protective layer 102 are located on the upper and lower surfaces of the lithium-replenishing composite diaphragm 1 as a whole, which plays a certain protective role on each membrane layer inside the lithium-replenishing composite diaphragm 1. At the same time, the manufacturing process of the second protective layer is simplified, and the overall preparation efficiency of the lithium-replenishing composite diaphragm 1 is improved.

[0116] In some other embodiments, as shown in Figure 5, based on the above embodiments, the lithium-supplementing composite diaphragm also includes a first protective layer 105, a second protective layer 102 and a third protective layer 106, that is, the lithium-supplementing composite diaphragm includes the third protective layer 106, the diaphragm layer 101, the second protective layer 102, the metallic lithium layer 103, the electronic conductive layer 104 and the first protective layer 105 in sequence. By providing three protective layers, the risk of exposure of the metallic lithium layer is further reduced to avoid partial or complete exposure of the metallic lithium layer 103 to air, water-containing air and / or water.

[0117] The embodiment of the present application also provides a lithium battery, as shown in FIG6 , which includes a positive electrode layer 4, a negative electrode layer 3, an electrolyte, and the lithium-supplementing composite separator 1 as described in the embodiment shown in FIG3 above. The positive electrode layer 4 includes a positive electrode current collector layer 401 and a positive electrode active material layer 402, and the negative electrode layer 3 includes a negative electrode current collector layer 301 and a negative electrode active material layer 302. The material of the positive electrode active material layer 402 is a ternary material (nickel (Ni), cobalt (Co), manganese (Mn), referred to as NCM), and can also be lithium cobalt oxide (chemical formula: LiCoO2, referred to as LCO), lithium iron phosphate (chemical formula: LiFePO4, referred to as LFP), lithium manganese oxide (chemical formula: LiMn2O4, referred to as LMO), lithium nickel manganese oxide (chemical formula can be expressed as LiNi 0.5 Mn 1.5O4, referred to as LMNO), and ternary materials (nickel (Ni), cobalt (Co), aluminum (Al, referred to as NCA) materials or other positive electrode materials one or more; the material of the negative electrode active material layer 302 is a graphite material, and can also be one or more of a silicon material, a silicon-carbon material, a silicon oxide material, a soft carbon material, a hard carbon material, an intermediate phase carbon microbead material or other negative electrode materials.

[0118] The present application also provides a lithium battery, as shown in FIG7 , which includes a positive electrode layer 4, a negative electrode layer 3, an electrolyte, and the lithium-supplementing composite separator 1 described in the embodiment shown in FIG4 . The positive electrode layer 4 includes a positive electrode current collector layer 401 and a positive electrode active material layer 402, and the negative electrode layer 3 includes a negative electrode current collector layer 301 and a negative electrode active material layer 302. The material of the positive electrode active material layer 402 is a ternary (NCM) material, and may also be one or more of lithium cobalt oxide (LCO), lithium iron phosphate (LFP), lithium manganese oxide (LMO), lithium nickel manganese oxide (LMNO), a ternary (NCA) material, or other positive electrode materials; the material of the negative electrode active material layer 302 is a graphite material, and may also be one or more of silicon material, silicon-carbon material, silicon oxide material, soft carbon material, hard carbon material, mesophase carbon microbead material, or other negative electrode materials.

[0119] The present invention provides a method for preparing a lithium-supplementing composite diaphragm, as shown in FIG8 , comprising the following steps:

[0120] Step S1: providing a diaphragm layer;

[0121] Step S2: forming a metallic lithium layer on one side of the separator layer;

[0122] Step S3: forming an electronic conductive layer on the surface of the metallic lithium layer;

[0123] Step S4: forming a first protective layer on the surface of the metallic lithium layer, wherein the orthographic projections of the electronic conductive layer and the first protective layer on the metallic lithium layer do not overlap or partially overlap.

[0124] In some embodiments, in step S2 , forming the metallic lithium layer on one side of the diaphragm layer includes: forming a second protective layer on one side of the diaphragm layer; and forming the metallic lithium layer on a surface of the second protective layer.

[0125] In some embodiments, in step S2 , forming the metallic lithium layer on one side of the diaphragm layer includes: forming a second protective layer on one side of the diaphragm layer; and forming the metallic lithium layer on a side of the diaphragm layer opposite to the second protective layer.

[0126] In some embodiments, a method for forming the first protective layer and / or the second protective layer includes at least one of the following:

[0127] Doctor coating, roller coating, spray coating, chemical vapor deposition, plasma vapor deposition, atomic layer deposition, pulsed laser deposition, vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering.

[0128] In some embodiments, the electronic conductive layer is formed by at least one of doctor blading, roller coating, spray coating, chemical vapor deposition, plasma vapor deposition, atomic layer deposition, pulsed laser deposition, vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering, or reactive sputtering.

[0129] In some embodiments, the method of forming the metallic lithium layer includes at least one of the following: vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering, or reactive sputtering.

[0130] The present invention provides a method for preparing a lithium battery, as shown in FIG9 , comprising the following steps:

[0131] Step S11: preparing a negative electrode for a lithium battery, wherein the negative electrode for the lithium battery comprises a negative electrode current collector layer and a negative electrode active material layer covering the negative electrode current collector layer;

[0132] Step S12: preparing a positive electrode of a lithium battery, wherein the positive electrode of the lithium battery includes a positive electrode current collector layer and a positive electrode active material layer covering the positive electrode current collector layer;

[0133] Step S13: preparing a lithium-supplementing composite diaphragm, wherein the preparation method of the lithium-supplementing composite diaphragm adopts any one of the methods described above:

[0134] Step S14: assembling the lithium-supplementing composite separator between the negative electrode and the positive electrode of the lithium battery so that the electronic conductive layer is attached to the negative electrode active material layer.

[0135] Comparative Example 1:

[0136] This comparative example provides a method for preparing a ceramic coating diaphragm and a lithium battery, comprising the following steps:

[0137] (1) preparing a positive electrode for a lithium-ion battery, wherein the positive electrode for the lithium-ion battery comprises a positive electrode current collector and an active material layer covering a surface of the positive electrode current collector;

[0138] (2) preparing a negative electrode for a lithium-ion battery, wherein the negative electrode for the lithium-ion battery comprises a negative electrode current collector and an active material layer covering a surface of the negative electrode current collector;

[0139] (3) Lithium battery production: The positive electrode and negative electrode obtained in step (1) and step (2) are assembled with an alumina ceramic coating separator into a battery for testing.

[0140] Comparative Example 2:

[0141] This comparative example provides a method for preparing a lithium-supplemented negative electrode sheet and a lithium battery, comprising the following steps:

[0142] (1) preparing a negative electrode for a lithium-ion battery, wherein the negative electrode for the lithium-ion battery comprises a negative electrode current collector and an active material layer covering a surface of the negative electrode current collector;

[0143] (2) preparing a lithium-supplemented negative electrode, by depositing a lithium layer on the surface of the active material of the negative electrode of the battery by magnetron sputtering technology on the negative electrode of the battery obtained in step (1), wherein the lithium layer is metallic lithium and the thickness of the deposited metallic lithium is 1000 nm;

[0144] (3) On the surface of the metallic lithium layer of the lithium-supplemented negative electrode obtained in step (2), a protective layer of Li2CO3 with a thickness of 30 nm is formed;

[0145] (4) preparing a positive electrode for a lithium-ion battery, wherein the positive electrode for the lithium-ion battery comprises a positive electrode current collector and an active material layer covering a surface of the positive electrode current collector;

[0146] (5) Assemble the lithium-supplemented negative electrode sheet and positive electrode sheet obtained in step (3) and step (4) with the alumina ceramic coating diaphragm into a battery for testing.

[0147] Comparative Example 3:

[0148] This embodiment provides a lithium-supplementing composite diaphragm and a method for preparing a lithium battery, comprising the following steps:

[0149] (1) preparing a lithium-supplemented composite diaphragm by depositing a metallic lithium layer on the surface of an alumina ceramic coating diaphragm using a vacuum evaporation technique, wherein the thickness of the deposited metallic lithium layer is 1000 nm;

[0150] (2) forming a first protective layer on the surface of the metal lithium layer of the lithium-supplementing composite diaphragm obtained in step (1), wherein the material is Li2CO3 and the thickness is 30 nm;

[0151] (3) preparing a positive electrode layer of a lithium-ion battery, wherein the positive electrode layer of the lithium-ion battery includes a positive electrode current collector layer and a positive electrode active material layer covering the surface of the positive electrode current collector layer;

[0152] (4) preparing a negative electrode layer of a lithium ion battery, wherein the negative electrode layer of the lithium ion battery includes a negative electrode current collector layer and a negative electrode active material layer covering the surface of the negative electrode current collector layer;

[0153] (5) Assemble the lithium-supplementing composite diaphragm, positive electrode layer, and negative electrode layer obtained in steps (2), (3), and (4) into a battery for testing.

[0154] Comparative Example 4:

[0155] This embodiment provides a lithium-supplementing composite diaphragm and a method for preparing a lithium battery, comprising the following steps:

[0156] (1) A lithium-supplemented composite diaphragm was prepared by depositing a second protective layer of LiPON with a thickness of 100 nm on the surface of the alumina ceramic coating diaphragm using magnetron sputtering technology;

[0157] (2) depositing a metallic lithium layer on the surface of the second protective layer of the lithium-supplementing composite diaphragm obtained in step (1) using a vacuum evaporation technique on the surface of the alumina ceramic coating diaphragm, wherein the thickness of the deposited metallic lithium layer is 1000 nm;

[0158] (3) forming a first protective layer on the surface of the metal lithium layer of the lithium-supplementing composite diaphragm obtained in step (2), wherein the material is Li2CO3 and the thickness is 30 nm;

[0159] (4) preparing a positive electrode layer of a lithium-ion battery, wherein the positive electrode layer of the lithium-ion battery includes a positive electrode current collector layer and a positive electrode active material layer covering the surface of the positive electrode current collector layer;

[0160] (5) preparing a negative electrode layer of a lithium ion battery, wherein the negative electrode layer of the lithium ion battery includes a negative electrode current collector layer and a negative electrode active material layer covering the surface of the negative electrode current collector layer;

[0161] (6) Assemble the lithium-supplementing composite diaphragm, positive electrode layer, and negative electrode layer obtained in steps (3), (4), and (5) into a battery for testing.

[0162] Example 1:

[0163] This embodiment provides a lithium-supplementing composite diaphragm and a method for preparing a lithium battery, comprising the following steps:

[0164] (1) preparing a lithium-supplemented composite diaphragm by depositing a metallic lithium layer on the surface of an alumina ceramic coating diaphragm using a vacuum evaporation technique, wherein the thickness of the deposited metallic lithium layer is 1000 nm;

[0165] (2) On the surface of the metal lithium layer of the lithium-supplementing composite diaphragm obtained in step (1), an electronic conductive layer is deposited on the surface of the metal lithium layer using magnetron sputtering technology. The material is silver, and the coverage rate of the electronic conductive layer on the metal lithium layer is 30%. The average area of ​​a single conductive unit of the multiple conductive units in the electronic conductive layer is 2500nm. 2 ;

[0166] (3) forming a first protective layer on the surface of the metal lithium layer of the lithium-supplementing composite diaphragm obtained in step (2), wherein the material is Li2CO3 and the thickness is 30 nm;

[0167] (4) preparing a positive electrode layer of a lithium-ion battery, wherein the positive electrode layer of the lithium-ion battery includes a positive electrode current collector layer and a positive electrode active material layer covering the surface of the positive electrode current collector layer;

[0168] (5) preparing a negative electrode layer of a lithium ion battery, wherein the negative electrode layer of the lithium ion battery includes a negative electrode current collector layer and a negative electrode active material layer covering the surface of the negative electrode current collector layer;

[0169] (6) Assemble the lithium-supplementing composite diaphragm, positive electrode layer, and negative electrode layer obtained in steps (3), (4), and (5) into a battery for testing.

[0170] Example 2:

[0171] This embodiment provides a method for preparing a lithium-supplementing composite diaphragm and a lithium battery, comprising the following steps:

[0172] (1) A lithium-supplemented composite diaphragm was prepared by depositing a second protective layer on the surface of the alumina ceramic coating diaphragm using magnetron sputtering technology. The material was LiPON with a thickness of 100 nm.

[0173] (2) depositing a metallic lithium layer on the surface of the second protective layer of the lithium-supplementing composite diaphragm obtained in step (1) using a vacuum evaporation technique on the surface of the alumina ceramic coating diaphragm, wherein the thickness of the deposited metallic lithium layer is 1000 nm;

[0174] (3) On the surface of the metal lithium layer of the lithium-supplementing composite diaphragm obtained in step (2), an electronic conductive layer is deposited on the surface of the metal lithium layer using magnetron sputtering technology. The material is silver, and the coverage rate of the electronic conductive layer on the metal lithium layer is 30%. The average area of ​​a single conductive unit of the multiple conductive units in the electronic conductive layer is 2500nm. 2 ;

[0175] (4) forming a first protective layer on the surface of the metal lithium layer of the lithium-supplementing composite diaphragm obtained in step (3), wherein the material is Li2CO3 and the thickness is 30 nm;

[0176] (5) preparing a positive electrode layer of a lithium-ion battery, wherein the positive electrode layer of the lithium-ion battery includes a positive electrode current collector layer and a positive electrode active material layer covering the surface of the positive electrode current collector layer;

[0177] (6) preparing a negative electrode layer of a lithium ion battery, wherein the negative electrode layer of the lithium ion battery includes a negative electrode current collector layer and a negative electrode active material layer covering the surface of the negative electrode current collector layer;

[0178] (7) Assemble the lithium-supplementing composite diaphragm, positive electrode layer, and negative electrode layer obtained in steps (3), (4), and (5) into a battery for testing.

[0179] Example 3:

[0180] This embodiment provides a method for preparing a lithium-supplementing composite diaphragm and a lithium battery, comprising the following steps:

[0181] (1) The lithium supplemented diaphragm obtained in step (3) of Example 1 was stored in a dry air environment for 30 days;

[0182] (2) preparing a positive electrode layer of a lithium-ion battery, wherein the positive electrode layer of the lithium-ion battery includes a positive electrode current collector layer and a positive electrode active material layer covering the surface of the positive electrode current collector layer;

[0183] (3) preparing a negative electrode layer of a lithium ion battery, wherein the negative electrode layer of the lithium ion battery includes a negative electrode current collector layer and a negative electrode active material layer covering the surface of the negative electrode current collector layer;

[0184] (4) Assembling the lithium-supplementing composite diaphragm, positive electrode layer, and negative electrode layer obtained in step (1), step (2), and step (3) into a battery for testing.

[0185] Example 4:

[0186] This embodiment provides a method for preparing a lithium-supplementing composite diaphragm and a lithium battery, comprising the following steps:

[0187] (1) The lithium supplemented diaphragm obtained in step (4) of Example 2 was stored in a dry air environment for 30 days;

[0188] (2) preparing a positive electrode layer of a lithium-ion battery, wherein the positive electrode layer of the lithium-ion battery includes a positive electrode current collector layer and a positive electrode active material layer covering the surface of the positive electrode current collector layer;

[0189] (3) preparing a negative electrode layer of a lithium ion battery, wherein the negative electrode layer of the lithium ion battery includes a negative electrode current collector layer and a negative electrode active material layer covering the surface of the negative electrode current collector layer;

[0190] (4) Assembling the lithium-supplementing composite diaphragm, positive electrode layer, and negative electrode layer obtained in step (1), step (2), and step (3) into a battery for testing.

[0191] The test data of the lithium batteries obtained in Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4, Example 1, Example 2, Example 3, and Example 4 are compared. The specific data are summarized in Table 1, the open circuit voltage change curve is shown in Figure 10, and the first charge and discharge curve is shown in Figure 11.

[0192] Table 1 Comparison of battery test data between comparative example and embodiment

[0193] By comparing the battery test data in Table 1 and the open circuit voltage change curve in Figure 10, it can be seen that the initial open circuit voltage of Comparative Example 1 is basically stable at about 0.26V, the initial open circuit voltage of Comparative Example 2 is basically stable at about 2.89V, the initial open circuit voltage of Comparative Example 3 is basically stable at about 3.11V, and the initial open circuit voltage of Comparative Example 4 is basically stable at about 3.08V. The initial open circuit voltage of Example 1 is 3.26V, and the initial open circuit voltage of Example 2 is 3.24V. It can be seen that the initial open circuit voltage of Examples 1-2 after using the lithium supplementation separator is significantly improved, and even compared with Comparative Examples 3 and Comparative Examples 4, the initial open circuit voltage is improved to a certain extent. After using the lithium-supplementing diaphragm of Comparative Examples 3-4 (without an electronic conductive layer), the initial open circuit voltage has a slow rising stage in the initial period of time, about 10 hours, and then tends to be stable. After using the lithium-supplementing diaphragm described in Examples 1-2 (with an electronic conductive layer), a stable initial open circuit voltage is reached within 3 hours. Therefore, after the lithium-supplementing composite diaphragm produced in Examples 1-2 of the present application is assembled into a lithium battery, the pre-lithiation behavior has begun before the charge and discharge test. When there is an electronic conductive layer, the pre-lithiation speed is significantly improved.

[0194] By comparing the battery test data in Table 1 and the first charge and discharge curves in Figure 11, it can be seen that the first coulombic efficiency of Comparative Example 1 is 89.2%, the first coulombic efficiency of Comparative Example 2 is 91.9%, the first coulombic efficiency of Comparative Example 3 is 93.7%, the first coulombic efficiency of Comparative Example 4 is 93.7%, the first coulombic efficiency of Example 1 is 94.3%, and the first coulombic efficiency of Example 2 is 94.3%. It can be seen that the lithium-supplementing composite separators manufactured in Examples 1-2 of the present application can effectively improve the first coulombic efficiency of lithium batteries, and when there is an electronic conductive layer, the first coulombic efficiency is the highest, and the utilization rate of the metallic lithium layer can be significantly improved.

[0195] By comparing the battery test data in Table 1 and the first charge and discharge curves in Figure 11, it can be seen that for Comparative Example 2, the first coulombic efficiency is 91.9%, and the utilization rate of the metal lithium layer is 26.1%; for Comparative Example 3, the first coulombic efficiency is 93.7%, and the utilization rate of the metal lithium layer is 44.1%; for Comparative Example 4, the first coulombic efficiency is 93.7%, and the utilization rate of the metal lithium layer is 44.1%; for Example 1, the first coulombic efficiency is 94.3%, and the utilization rate of the metal lithium layer is 49.3%; for Example 2, the first coulombic efficiency is 94.3%, and the utilization rate of the metal lithium layer is 49.3%; it can be seen that in terms of the improvement of the first efficiency of the lithium battery and the utilization rate of the metal lithium layer, the lithium-replenishing composite diaphragms manufactured by Examples 1-2 of the present application are superior to the lithium-replenishing negative electrode sheets manufactured by Comparative Examples 2-4, and are particularly superior to the lithium-replenishing negative electrode sheets manufactured by Comparative Example 2.

[0196] The composite diaphragm obtained in Example 1 and the composite diaphragm obtained in Example 2 were placed under the same conditions. The initial state of the diaphragms was compared as shown in FIG12 . After 15 days of placement, the comparison state of the diaphragms was shown in FIG13 . After 30 days of placement, the comparison state of the diaphragms was shown in FIG14 .

[0197] By comparing FIG12 with FIG13 , it can be seen that the state changes of the lithium-supplemented composite diaphragm obtained in Example 1 and the lithium-supplemented composite diaphragm obtained in Example 2 are as follows: after being set aside for 15 days, the metallic lithium layer of the lithium-supplemented composite diaphragm of Example 1 has undergone many side reactions, and a large number of dark spots appear on the surface of the diaphragm, as indicated by the arrows in FIG13 , while the metallic lithium layer of the lithium-supplemented composite diaphragm of Example 2 has no dark spots, indicating that no side reactions have occurred, or very few side reactions have occurred;

[0198] By comparing Figure 12 with Figure 14, it can be seen that the state changes of the lithium-supplemented composite diaphragm obtained in Example 1 and the lithium-supplemented composite diaphragm obtained in Example 2 are that after being left for 30 days, the metallic lithium layer of the lithium-supplemented composite diaphragm of Example 1 has been completely consumed by side reactions, while the metallic lithium layer of the lithium-supplemented composite diaphragm of Example 2 has only a small amount of side reactions, and only a small amount of dark spots appear on the surface of the diaphragm.

[0199] By comparing the battery test data in Table 1 with the open circuit voltage change curve after 30 days of storage in Figure 15, it can be seen that the initial open circuit voltage of Comparative Example 1 is basically stable at around 0.26V, and the initial open circuit voltage of Example 3 is 0.36V, which is not much different from the initial open circuit voltage of Comparative Example 1; while the initial open circuit voltage of Example 4 is 3.23V, which is significantly higher than the initial open circuit voltages of Comparative Example 1 and Example 3. This indicates that after 30 days of storage, the lithium-supplemented composite separator of Example 4, after being assembled into a lithium battery, still exhibits pre-lithiation behavior before charge and discharge testing.

[0200] By comparing the battery data in Table 1, it can be seen that the first coulombic efficiency of Example 3 is 89.5%, and the utilization rate of the metal lithium layer is 0%; the first coulombic efficiency of Example 4 is 92.2%, and the utilization rate of the metal lithium layer is 29.5%; it can be seen that the pre-lithiation composite diaphragm with a second protective layer can still be pre-lithiated after storage for 30 days.

[0201] This shows that in Examples 2 and 4 with the second protective layer, the provision of the second protective layer can significantly protect the metallic lithium layer, thereby improving the storage life and service life of the lithium-supplementing composite diaphragm and reducing the requirements of the lithium-supplementing composite diaphragm for storage conditions and usage conditions.

[0202] Comparison of the room temperature cycle curves in Figure 16 shows that after 80 cycles, the discharge capacity retention rates of Examples 1-2 of the present application are all higher than those of Comparative Examples 1-4. This shows that the composite lithium-supplementing separators produced in Examples 1-2 of the present application can effectively improve the cycling performance of lithium batteries.

[0203] A comparison of the room temperature cycle curves in Figure 16 shows that the curves of Examples 1-2 of the present application are significantly higher than those of Comparative Examples 1-4, indicating that the cycle performance of Examples 1-2 of the present application is significantly better than that of Comparative Example 2. It can be seen that in terms of improved battery cycle performance, the composite lithium-supplementing separators manufactured in Examples 1-2 of the present application are superior to the lithium-supplementing negative electrode sheets of Comparative Examples 1-4.

[0204] A comparison of the room-temperature cycle curves of Comparative Examples 3 and 4, and the room-temperature cycle curves of Examples 1 and 2 in Figure 16 shows that the curves for Comparative Examples 3 and 4 are essentially identical, and the curves for Examples 1 and 2 are also essentially identical, with no significant differences. This indicates that the second protective layer has no significant adverse effect on the battery's cycling performance.

[0205] By comparing the room temperature cycle curves of Comparative Example 3 and Example 1, and comparing the room temperature cycle curves of Comparative Example 4 and Example 2 in Figure 16, it can be seen that the curve of Example 1 is significantly higher than the curve of Comparative Example 3, and the curve of Example 2 is also significantly higher than the curve of Comparative Example 4, indicating that the cycle performance of Example 1 is significantly better than that of Comparative Example 3, and the cycle performance of Example 2 is significantly higher than that of Comparative Example 4. It can be seen that the lithium-supplementing composite separator manufactured in this application can further improve the cycle performance of the battery when it has an electronic conductive layer.

[0206] The lithium-replenishing composite diaphragm of the present application can be directly applied to the negative electrode lithium replenishment, thereby improving the initial coulombic efficiency and cycle life of the lithium battery. The lithium-replenishing composite diaphragm of the present application can control the degree of lithium replenishment (pre-lithiation) by regulating the thickness of the lithium layer, and improves the utilization rate of lithium in the pre-lithiation process. The composite diaphragm of the present application provides an electronic conductive channel between the lithium layer and the negative electrode active material, thereby reducing the generation of dead lithium and further improving the utilization rate of lithium. The lithium-replenishing composite diaphragm of the present application also has the feature of not changing the normal production process flow of the lithium battery, thereby not reducing the production efficiency of the lithium battery. The lithium-replenishing composite diaphragm of the present application has a protective layer on both sides of the lithium layer, which isolates the lithium layer from the external environment, so that the lithium layer does not react with the air and water in the environment, so the lithium-replenishing composite diaphragm has relatively low requirements for the storage environment. In addition, the lithium-supplementing composite diaphragm of the present application provides an electronic conductive path and an ion conductive path between the lithium layer and the negative electrode active material. After the battery is assembled, a solid electrolyte film (SEI) can be formed in situ, further reducing the loss of active lithium and improving the coulombic efficiency and cycle life of the lithium battery.

[0207] Finally, it should be noted that the various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0208] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A lithium-supplementing composite diaphragm for a lithium battery, wherein the lithium battery comprises a negative electrode layer and a positive electrode layer, and the lithium-supplementing composite diaphragm is arranged between the negative electrode layer and the positive electrode layer, characterized in that: The lithium-supplementing composite diaphragm comprises: a separator layer configured to separate the negative electrode layer from the positive electrode layer; A metal lithium layer, disposed on a side of the separator layer close to the negative electrode layer, configured to supplement lithium to the negative electrode layer; A first protective layer is disposed on a side of the metal lithium layer close to the negative electrode layer; An electronic conductive layer, disposed on a side of the metal lithium layer close to the negative electrode layer, configured to provide an electronic conductive channel between the metal lithium layer and the negative electrode layer; The electronic conductive layer and the first protective layer partially overlap the orthographic projection of the metal lithium layer, so that there is no gap between the electronic conductive layer and the first protective layer, thereby ensuring that the electronic conductive layer and the first protective layer can completely cover the metal lithium layer 100%; The material of the first protective layer includes at least one of the following: Al2O3, MgO, ZnO2, TiO2, ZrO2, LaO2, CeO2, Y2O3, Si x O, SiC, SiN x 、SiCN x , AlN, Mg(OH)2, BaSO4, boehmite or perovskite; or, <h2 style=";text-align:left;direction:ltr">Li2CO3、Li3N、LiF、Li3PO4、Li4SiO4、Li4Ti5O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> 、LiPON、LiSiON、LLZO、LLZTO、LATP、Li3Fe2(PO4)3、Li3V2(PO4)3、Li3In2(PO4)3、Li3Sc2(PO4)3、Li3Cr2(PO4)3; The method for forming the first protective layer includes at least one of the following: scraping, roller coating, spraying, chemical vapor deposition, plasma vapor deposition, atomic layer deposition, pulsed laser deposition, vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering.

2. The lithium-supplementing composite diaphragm according to claim 1, characterized in that: The lithium-supplementing composite diaphragm also includes: The second protective layer is arranged on a side of the metal lithium layer away from the negative electrode layer.

3. The lithium-supplementing composite diaphragm according to claim 1, characterized in that: The lithium-supplementing composite diaphragm also includes: The second protective layer is arranged on a side of the diaphragm layer away from the metal lithium layer.

4. The lithium-supplementing composite diaphragm according to claim 1, characterized in that: The orthographic projection shape of the electronic conductive layer on the metal lithium layer is an island shape, wherein the island shape includes a plurality of discontinuous island shapes and / or at least one network shape formed by connecting a plurality of island shapes.

5. The lithium-supplementing composite diaphragm according to claim 1, characterized in that: The thickness of the electron conductive layer is greater than the thickness of the first protective layer.

6. The lithium-supplementing composite diaphragm according to claim 1, characterized in that: The thickness of the electronic conductive layer is 10nm-1000nm.

7. The lithium-supplementing composite diaphragm according to claim 1, characterized in that: The coverage rate of the electronic conductive layer on the metal lithium layer is 10%-90%.

8. The lithium-supplementing composite diaphragm according to claim 1, characterized in that: The area of ​​a single electronic conductive layer is 100 nm 2 ~1000000nm 2 .

9. The lithium-supplementing composite diaphragm according to claim 2 or 3, characterized in that: The thickness of the first protective layer and / or the second protective layer is 10nm-1000nm.

10. The lithium-supplementing composite diaphragm according to claim 1, characterized in that: The thickness of the metal lithium layer is 0.1 μm-10 μm, and the metal lithium layer is a dense or porous loose structure.

11. The lithium-supplementing composite diaphragm according to claim 1, characterized in that: The material of the electronic conductive layer includes at least one of the following: metal, metal oxide, metal nitride, metal sulfide or carbon material.

12. The lithium-supplementing composite diaphragm according to claim 11, characterized in that: The metal material includes at least one of the following: gold, silver, copper, iron, titanium, aluminum, manganese, tin, cobalt, nickel, chromium, bismuth, vanadium, molybdenum or niobium; The carbon material includes at least one of the following: graphite, hard carbon, soft carbon, graphene or carbon nanotube.

13. The lithium-supplementing composite diaphragm according to claim 2 or 3, characterized in that: The material of the second protective layer includes at least one of the following: Al2O3, MgO, ZnO2, TiO2, ZrO2, LaO2, CeO2, Y2O3, Si x O, SiC, SiN x 、SiCN x , AlN, Mg(OH)2, BaSO4, boehmite or perovskite; or, <h2 style=";text-align:left;direction:ltr">Li2CO3、Li3N、LiF、Li3PO4、Li4SiO4、Li4Ti5O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> 、LiPON、LiSiON、LLZO、LLZTO、LATP、Li3Fe2(PO4)3、Li3V2(PO4)3、Li3In2(PO4)3、Li3Sc2(PO4)3、Li3Cr2(PO4)3。 14. The lithium-supplementing composite diaphragm according to claim 1, characterized in that: The diaphragm layer is one of the following: a base membrane, a base membrane / ceramic composite diaphragm, a base membrane / adhesive composite diaphragm, and a base membrane / ceramic / adhesive composite diaphragm.

15. The lithium-supplementing composite diaphragm according to claim 14, characterized in that: The base film comprises at least one of the following: a polyethylene base film, a polyethylene non-woven base film, a polypropylene base film, a polypropylene non-woven base film, a polypropylene / polyethylene / polypropylene composite base film, a polyimide base film, a polyimide non-woven base film, a polytetrafluoroethylene base film, a polytetrafluoroethylene non-woven base film, a polyvinyl chloride base film or a polyvinyl chloride non-woven base film; and / or, The ceramic comprises at least one of the following: alumina, zirconium oxide, boehmite, magnesium hydroxide, barium sulfate, silicon oxide, aluminum nitride, magnesium oxide, titanium dioxide, yttrium oxide or cerium oxide; and / or, The adhesive comprises at least one of the following: polytetrafluoroethylene, polyvinylidene fluoride, acrylic acid, polyethylene oxide, sodium carboxymethyl cellulose, styrene-butadiene rubber, hydroxypropyl methyl cellulose, carboxy styrene-butadiene latex or polyvinyl alcohol.

16. The lithium-supplementing composite diaphragm according to claim 1, characterized in that: The metallic lithium layer includes at least one of the following: metallic lithium, lithium silicon alloy, lithium tin alloy, lithium magnesium alloy, lithium copper alloy, lithium silver alloy, lithium beryllium alloy, lithium zinc alloy, lithium cadmium alloy, lithium aluminum alloy, lithium gold alloy and lithium boron alloy.

17. A lithium battery, characterized in that: A lithium-supplementing composite separator comprising any one of claims 1 to 16, wherein the negative electrode layer comprises a negative electrode current collector layer and a negative electrode active material layer covering the negative electrode current collector layer; and the positive electrode layer comprises a positive electrode current collector layer and a positive electrode active material layer covering the positive electrode current collector layer.

18. A method for preparing the lithium-supplementing composite diaphragm according to any one of claims 1 to 16, characterized in that: The following steps are involved: providing a diaphragm layer; forming a metallic lithium layer on one side of the separator layer; forming an electronic conductive layer on the surface of the metallic lithium layer; A first protective layer is formed on the surface of the metal lithium layer, wherein the electronic conductive layer and the first protective layer partially overlap at the orthographic projection of the metal lithium layer.

19. The method according to claim 18, characterized in that The forming of a metallic lithium layer on one side of the diaphragm layer comprises: forming a second protective layer on one side of the diaphragm layer; A metal lithium layer is formed on the surface of the second protective layer.

20. The method according to claim 18, characterized in that The forming of a metallic lithium layer on one side of the diaphragm layer comprises: forming a second protective layer on one side of the diaphragm layer; A metal lithium layer is formed on a side of the separator layer opposite to the second protective layer.

21. The method according to claim 19 or 20, characterized in that The method for forming the second protective layer includes at least one of the following: Doctor coating, roller coating, spray coating, gravure coating, extrusion coating, screen printing, chemical vapor deposition, plasma vapor deposition, atomic layer deposition, pulsed laser deposition, vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering.

22. The method according to claim 18, characterized in that The method for forming the electronic conductive layer includes at least one of the following: scraping, roller coating, spraying, chemical vapor deposition, plasma vapor deposition, atomic layer deposition, pulsed laser deposition, vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering.

23. The method according to claim 18, characterized in that The method for forming the metal lithium layer comprises at least one of the following: Vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering.

24. A method for preparing a lithium battery, characterized in that: The following steps are involved: Prepare a negative electrode for a lithium battery, wherein the negative electrode for the lithium battery comprises a negative electrode current collector layer and a negative electrode active material layer covering the negative electrode current collector layer; Prepare a positive electrode for a lithium battery, wherein the positive electrode for the lithium battery comprises a positive electrode current collector layer and a positive electrode active material layer covering the positive electrode current collector layer; Prepare a lithium-supplemented composite diaphragm, wherein the preparation method of the lithium-supplemented composite diaphragm adopts the method according to any one of claims 18 to 23; The lithium-supplementing composite separator is assembled between the negative electrode and the positive electrode of the lithium battery, so that the electronic conductive layer is attached to the negative electrode active material layer.

Citation Information

Patent Citations

  • Lithium supplementing diaphragm of lithium ion battery

    CN110676420A

  • Composite diaphragm with lithium supplementing effect, and preparation method thereof and lithium ion battery

    CN112599928A

  • Pre-lithiated negative plate, preparation method thereof and lithium battery

    CN114335417A

  • Lithium supplement composite diaphragm for lithium battery, lithium battery and preparation method of lithium supplement composite diaphragm

    CN116053708A

  • Surface-stabilized and prelithiated anode active materials for lithium batteries and production method

    US20190088930A1

Cited By

  • Asymmetric functional sodium battery diaphragm as well as preparation method and application thereof

    CN119833880A