Positive electrode material, secondary battery, and electrical device
By coating the surface of the sodium-ion battery cathode material with electronic conductors and ion conductors to form a dense layer, the problem of low conductivity is solved, the electrochemical performance and stability of the battery are improved, and it is suitable for industrial production.
Patent Information
- Application Number
- PCT/CN2023/141710
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2023-12-25
- Publication Date
- 2024-10-03
AI Technical Summary
Existing sodium-ion battery cathode materials have low electronic conductivity and ionic conductivity, resulting in poor structural stability and rate characteristics.
Part of the surface of the cathode active material is coated with electronic conductors and ionic conductors to control the particle size ratio and form a dense coating layer to improve conductivity and interface ion transmission effects. The ionic conductors are used to remove HF in the electrolyte and reduce corrosion. .
It significantly improves the electronic conductivity and ion conductivity of the cathode material, enhances the electrochemical performance and stability of the battery, simplifies the production process, and facilitates industrial application.
Smart Images

Figure CN2023141710_03102024_PF_FP_ABST
Abstract
Description
Positive electrode material, secondary battery and electrical equipment
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese invention patent application CN202310361754.9 filed on March 31, 2023, the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present application relates to the field of new energy technology, and in particular to a positive electrode material, a secondary battery and an electrical device. Background Art
[0004] Secondary batteries, especially sodium-ion secondary batteries, are ideal substitutes for lithium-ion batteries due to their abundant sodium resources and low cost, and are receiving increasing attention in large-scale energy storage applications. The main cathode materials currently used for sodium-ion batteries include layered oxides, polyanion-type cathode active materials, etc. Among them, layered oxides used as cathode materials for sodium-ion batteries have the characteristics of high capacity, high voltage, and high energy density, but they also have inherent limitations, such as low electronic conductivity and poor interfacial ion transport properties, which lead to poor structural stability and rate characteristics. Polyanion-type cathode active materials have the characteristics of structural stability, high safety, and high operating voltage, but their electronic conductivity is low, resulting in very limited capacity.
[0005] How to improve the electronic conductivity and ionic conductivity of sodium ion battery positive electrode materials has become a technical problem that needs to be solved urgently.
[0006] Summary of the Invention
[0007] Based on the defects of the existing technology, the present application provides a positive electrode material, a secondary battery and an electrical device to effectively improve the electronic conductivity and ionic conductivity of the positive electrode material.
[0008] In a first aspect, the present application provides a positive electrode material, comprising a positive electrode active material and a coating material, wherein the coating material is distributed on at least a portion of the surface of the positive electrode active material;
[0009] The coating material comprises an electronic conductor and an ion conductor;
[0010] The ratio of the particle diameters Dv50 of the positive electrode active material and the electron conductor is 1:(0.01 to 0.25); and
[0011] The ratio of the particle diameters Dv50 of the positive electrode active material and the ion conductor is 1:(0.08-0.5).
[0012] Preferably, the particle size Dv50 of the ion conductor is 0.05 to 7.5 μm.
[0013] Preferably, the particle size Dv50 of the ion conductor is 0.5-5 μm.
[0014] Preferably, the ion conductor includes at least one of a first ion conductor and a second ion conductor, the first ion conductor having a Nasicon structure, and / or the second ion conductor having a layered structure.
[0015] Preferably, the first ion conductor comprises Na 3+Ax Zr 2-0.5Ax M x Si2PO 12 , wherein M is selected from at least one of Li, Ca, Mg, Sr, Ba, In, Ga, Nb, La, Cr, Mn, Zn, Al, Ge, and Bi, A is the valence state of the element M, and 0≤x≤0.5; and / or the second ion conductor includes Na y -β"-Al2O3, where 0 <y≤1。
[0016] Preferably, the mass ratio of the first ion conductor to the second ion conductor is 1:(0.16-6).
[0017] Preferably, the coating material further comprises a polymer, and the polymer comprises at least one of polyacrylonitrile, polyvinyl pyrrolidone, and polyethylene oxide.
[0018] Preferably, the mass of the polymer is 0.5% to 3% of the total mass of the coating material.
[0019] Preferably, the mass of the ion conductor is 10% to 90% of the total mass of the electron conductor and the ion conductor.
[0020] Preferably, the coating material has a thickness of 0.6 to 8 μm on the surface of the positive electrode active material.
[0021] Preferably, the positive electrode active material includes at least one of a layered oxide and a polyanionic positive electrode active material.
[0022] Preferably, the electron conductor comprises a carbon material.
[0023] Preferably, the mass ratio of the ion conductor to the positive electrode active material is 1:(10-500).
[0024] In a second aspect, the present application provides a secondary battery comprising the positive electrode material.
[0025] In a third aspect, the present application provides an electrical device, comprising the above-mentioned secondary battery, wherein the secondary battery serves as a power supply for the electrical device.
[0026] Compared with the prior art, the present invention has the following advantages:
[0027] (1) The present application coats at least part of the surface of the positive electrode active material with a coating material containing an electronic conductor and an ion conductor, thereby utilizing the coating of the electronic conductor to improve the conductivity of the positive electrode active material, utilizing the coating of the ion conductor to promote the interfacial ion transport effect, and utilizing the coating layer formed by the electronic conductor and the ion conductor to inhibit the phase change of the positive electrode active material during the electrochemical process, thereby improving its stability. In addition, the surface ion conductor can even effectively remove HF in the electrolyte, reduce the acid corrosion of the positive electrode active material during the electrochemical process, reduce the dissolution of transition metal ions, and further improve the stability of the positive electrode active material;
[0028] (2) The present application ensures that a dense coating layer is formed on the surface of the positive electrode active material by controlling the particle size Dv50 ratio of the positive electrode active material and the electronic conductor within the range of 1: (0.01 to 0.25) and the particle size Dv50 ratio of the positive electrode active material and the ion conductor within the range of 1: (0.08 to 0.5), so that the ion conductor is in close contact not only with the positive electrode active material to facilitate ion transmission, but also with the electronic conductor to facilitate electron transmission;
[0029] (3) This application effectively improves the electronic conductivity and ionic conductivity of the secondary battery positive electrode material, and the method is simple, which is convenient for industrial production and promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] FIG1 is a schematic structural diagram of the positive electrode materials of various embodiments and comparative examples;
[0031] Among them, 1-positive electrode active material, 2-coating material. DETAILED DESCRIPTION
[0032] In order to better illustrate the purpose, technical solutions and advantages of the present application, the present application will be further described below in conjunction with specific embodiments and comparative examples. Its purpose is to understand the content of the present application in detail, rather than to limit the present application. All other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present application. The experimental reagents and instruments involved in the implementation of this application are all commonly used ordinary reagents and instruments unless otherwise specified.
[0033] In this application, the particle size Dv50 refers to the particle size when the volume cumulative distribution in the sample particle size distribution is 50%.
[0034] (1) Cathode materials
[0035] According to a first aspect of the present application, there is provided a device comprising a positive electrode active material and a coating material, wherein the coating material is distributed on at least a portion of the surface of the positive electrode active material;
[0036] The coating material comprises an electronic conductor and an ion conductor;
[0037] The ratio of the particle size Dv50 of the positive electrode active material and the electron conductor is 1:(0.01-0.25);
[0038] The ratio of the particle diameters Dv50 of the positive electrode active material and the ion conductor is 1:(0.08-0.5).
[0039] In the present application, a coating material containing an electronic conductor and an ion conductor is coated on at least part of the surface of the positive electrode active material, so that the conductivity of the positive electrode active material is improved by coating with the electronic conductor, the interfacial ion transport effect is promoted by coating with the ion conductor, and the coating layer formed by the electronic conductor and the ion conductor is used to inhibit the phase change of the positive electrode active material during the electrochemical process, thereby improving its stability. In addition, the ion conductor on the surface can even effectively remove HF in the electrolyte, because the metal elements contained in the ion conductor can combine with the F element, reducing the generation of HF, thereby reducing the corrosion of the positive electrode active material by the acid during the electrochemical process, reducing the dissolution of transition metal ions, and further improving the stability of the positive electrode active material.
[0040] In practical applications, XPS argon ion etching can be used to etch away the coating material of the positive electrode active material layer, after which the Dv50 of the main positive electrode active material can be measured using a laser particle size analyzer. The main positive electrode active material can be dissolved with hydrochloric acid, retaining the ionic conductor and electronic conductor. Both can be calcined to remove the electronic conductor, allowing the Dv50 of the ionic conductor to be measured using a laser particle size analyzer. Alternatively, aqua regia can be used to remove the ionic conductor, retaining the electronic conductor, allowing the Dv50 of the electronic conductor to be measured using a laser particle size analyzer.
[0041] In the present application, by controlling the ratio of the particle size Dv50 of the positive electrode active material and the electronic conductor within the range of 1:(0.01 to 0.25) and the ratio of the particle size Dv50 of the positive electrode active material and the ion conductor within the range of 1:(0.08 to 0.5), a dense coating layer is ensured to be formed on the surface of the positive electrode active material, and the ion conductor is not only in close contact with the positive electrode active material to facilitate the transmission of ions, but also in close contact with the electronic conductor to facilitate the transmission of electrons. At the same time, the coating layer has suitable pore channels, which further improves the transmission efficiency of electrons and ions, thereby making the battery have better electrochemical performance, such as higher rate and better cycle stability.
[0042] In some embodiments, the particle size Dv50 of the ion conductor is 0.075 to 15 μm.
[0043] In some embodiments, the particle size Dv50 of the positive electrode active material is 5 to 80 μm.
[0044] In some embodiments, the particle size Dv50 of the electron conductor is 0.05 to 7.5 μm.
[0045] In some embodiments, the particle size Dv50 of the positive electrode active material is 5 to 80 μm, the particle size Dv50 of the electronic conductor is 0.05 to 7.5 μm, and the particle size Dv50 of the ion conductor is 0.075 to 15 μm.
[0046] The positive electrode material of the present application has high electronic conductivity and ionic conductivity, which effectively solves the technical problem of low electronic conductivity and ionic conductivity of secondary battery positive electrode materials in the prior art. In addition, the production method is simple, which is convenient for industrial production and promotion and application.
[0047] In some embodiments, the particle size Dv50 of the ion conductor is 0.5 to 5 μm. When the particle size of the ion conductor is distributed within the above range, it is beneficial to improve the density of the coating layer, thereby facilitating the transmission of ions and electrons.
[0048] In some embodiments, the ion conductor includes at least one of a first ion conductor and a second ion conductor, wherein the first ion conductor has a Nasicon structure and the second ion conductor has a layered structure. Both the first ion conductor and the second ion conductor have excellent ion conductivity and can effectively remove HF from the electrolyte, reducing acid corrosion of the positive electrode active material during the electrochemical process, reducing the dissolution of transition metal ions, and further improving the stability of the positive electrode active material.
[0049] In some specific embodiments, the ion conductor includes a first ion conductor and a second ion conductor, and the difference in particle shape structure and ion conduction characteristics between the first and second ion conductors is utilized to optimize ion transmission efficiency and reduce impedance. In some embodiments, the ion conductivity of the ion conductor is 1×10 -4 ~9×10 -3 S / cm.
[0050] In some embodiments, the first ion conductor comprises Na 3+Ax Zr 2-0.5Ax M x Si2PO 12 , wherein M is selected from at least one of Li, Ca, Mg, Sr, Ba, In, Ga, Nb, La, Cr, Mn, Zn, Al, Ge, and Bi, A is the valence state of the element M, and 0≤x≤0.5; and / or the second ion conductor includes Na y-β”-Al2O3, where 0 < y ≤ 1. In some specific embodiments, the mass ratio of the first ionic conductor to the second ionic conductor is 1:(0.16 - 6). The above-mentioned first ionic conductor and second ionic conductor have excellent ionic conduction performance, which is beneficial to reducing the material impedance value and improving the battery rate performance. In practical applications, the proportion of the first ionic conductor and the second ionic conductor can be accurately calculated by measuring the content of characteristic elements by ICP. For example, by quantitatively testing the Zr element in the first ionic conductor and the Al element in the second ionic conductor, the specific content and proportional relationship of the above two ionic conductors can be obtained.
[0051] In some embodiments, the coating material further includes a polymer, and the polymer includes at least one of polyacrylonitrile (PAN), polyvinylpyrrolidone (PVP), polyethylene oxide (PEO), etc., but the types of polymers are not limited thereto. In some specific embodiments, the mass of the polymer is from 0.5% to 3% of the total mass of the coating material. By adding a polymer to the coating material, the components in the coating material are bonded to make the coating layer denser.
[0052] In some embodiments, the positive electrode active material includes at least one of layered oxides and polyanionic positive electrode active materials.
[0053] In some embodiments, the crystal structure of the layered oxide includes at least one of the O3 phase and the P2 phase. The O3 phase has an open Na + channel, with high capacity, but its stability is poor. The P2 phase has a relatively high stable structure.
[0054] In some specific embodiments, the layered oxide includes Na x MO2, where x ≤ 1, and M is at least one of transition metals. M can be selected from at least one of Fe, Co, Ni, Mn, Ti, Cr, etc., but is not limited thereto. When x is in the range of 0.8 - 1, the crystal structure of Na x MO2 is the O3 phase; when x is in the range of 0.6 - 0.7, the crystal structure of Na x MO2 is the P2 phase.
[0055] In some specific embodiments, the polyanionic positive electrode active material includes Na3V2(PO4)3, but is not limited thereto.
[0056] In some embodiments, the mass of the ionic conductor is from 10% to 90% of the total mass of the electronic conductor and the ionic conductor. The mass of the ionic conductor is preferably from 30% to 50% of the total mass of the electronic conductor and the ionic conductor to further improve the electronic conductivity and ionic conductivity of the positive electrode material.
[0057] In some embodiments, the mass ratio of the ion conductor to the positive electrode active material is 1:(10-500). Preferably, the mass ratio of the ion conductor to the positive electrode active material is 1:(100-300). In some embodiments, the molar ratio of the ion conductor to the positive electrode active material is 1:300 to 1:10. A mass ratio within the above range ensures that the positive electrode material has better ion conductivity and helps ensure that the positive electrode material has lower impedance.
[0058] In some embodiments, the coating material has a thickness of 0.6 to 8 μm on the surface of the positive electrode active material. If the coating material is too thick, the battery efficiency will be low and the capacity will decay rapidly in the early stages of the cycle. If the coating material is too thin, the battery capacity and cycle performance will be adversely affected. Therefore, the thickness of the coating material on the surface of the positive electrode active material is controlled within the range of 0.6 to 8 μm.
[0059] In some embodiments, the electron conductor comprises a carbon material, which may be selected from at least one of hard carbon, soft carbon, graphene, carbon nanotubes, and graphene oxide, but is not limited thereto.
[0060] In some specific embodiments, the method for preparing the positive electrode material comprises the following steps:
[0061] Adding a sodium source, a zirconium source, a silicon source, a phosphorus source, a carbon source and a positive electrode active material into a solvent and dispersing them to obtain a precursor slurry;
[0062] The obtained precursor slurry is calcined under a protective gas atmosphere after removing the solvent to obtain the surface-coated Na3Zr2Si2PO 12and carbon materials to obtain a positive electrode active material. In some embodiments, the sodium source includes, but is not limited to, sodium acetate, sodium citrate, sodium carbonate, sodium bicarbonate, etc.; the zirconium source includes, but is not limited to, zirconium acetate, zirconium oxide, zirconium nitrate, zirconyl nitrate, etc.; the silicon source includes, but is not limited to, silicon dioxide, ethyl silicate, sodium silicate, etc.; the phosphorus source includes, but is not limited to, phosphoric acid, ammonium hydrogen phosphate, sodium phosphate, sodium hydrogen phosphate, etc.; and the carbon source includes, but is not limited to, glucose, sucrose, starch, polyacrylonitrile, polyvinyl alcohol, polyvinyl pyrrolidone, polymethyl methacrylate, etc. In some embodiments, the solvent includes, but is not limited to, water, ethanol, acetone, methanol, isopropanol, N-methylpyrrolidone, N,N-dimethylformamide, triethylene glycol, etc. When preparing the precursor slurry, the order of adding the raw materials is not limited, as long as the raw materials are evenly dispersed. In some specific embodiments, when preparing the precursor slurry, the sodium source, zirconium source, silicon source, and phosphorus source are first added to the solvent, dissolved, and then the carbon source is added. After dispersion, the positive electrode active material is added and dispersed to obtain the precursor slurry. This method is more conducive to evenly dispersing the raw materials. In some embodiments, after removing the solvent, the resulting precursor slurry can be directly calcined, or pre-calcined before calcining. In some embodiments, the pre-calcination temperature is between 200°C and 300°C, and the pre-calcination time is between 1 and 5 hours. In some embodiments, the calcination temperature is not less than 800°C, and the calcination time is greater than 1 hour.
[0063] In some specific embodiments, the method for preparing the positive electrode material comprises the following steps:
[0064] Aluminum source, sodium source and carbon source are added to a solvent, dissolved and then the solvent is removed and calcined to obtain Na-β"-Al2O3 blocks, which are then ground and sieved to obtain Na-β"-Al2O3 powder;
[0065] The obtained Na-β"-Al2O3 powder and carbon source are added to a solvent, dispersed, and then the positive electrode active material is added and dispersed to obtain a precursor slurry;
[0066] After removing the solvent from the resulting precursor slurry, the precursor slurry is calcined under a protective gas atmosphere to obtain a positive electrode active material coated with Na-β"-Al2O3 and a carbon material, namely, a positive electrode material. In some embodiments, the aluminum source includes but is not limited to aluminum chloride, aluminum nitrate, aluminum sulfate, etc.; the sodium source includes but is not limited to sodium chloride, sodium nitrate, sodium sulfate, etc.; the carbon source used to prepare the Na-β"-Al2O3 blocks and the precursor slurry includes but is not limited to glucose, sucrose, starch, polyacrylonitrile, polyvinyl alcohol, polyvinyl pyrrolidone, polymethyl methacrylate, etc. In some embodiments, the solvent used to prepare the Na-β"-Al2O3 blocks and the solvent used to prepare the precursor slurry include but are not limited to water, ethanol, acetone, methanol, isopropanol, N-methylpyrrolidone, N,N-dimethylformamide, triethylene glycol, etc. In some embodiments, the calcination temperature for preparing the Na-β"-Al2O3 blocks is not less than 800°C, and the calcination time is greater than 1 hour. In some embodiments, the calcination temperature for preparing the Na-β"-Al2O3 blocks is not less than 600°C, and the calcination time is greater than 1 hour. In some embodiments, the mass of the carbon source used to prepare the Na-β"-Al2O3 block accounts for 0.5-2% of the total mass of all carbon sources. It should be noted that these embodiments only consider the mass of Al2O3 and the hard carbon contained therein when calculating the mass of Na-β"-Al2O3 powder, and the same applies below.
[0067] In some specific embodiments, the method for preparing the positive electrode material comprises the following steps:
[0068] Aluminum source, sodium source and carbon source are added to a solvent, dissolved and then the solvent is removed and calcined to obtain Na-β"-Al2O3 blocks, which are then ground and sieved to obtain Na-β"-Al2O3 powder;
[0069] The obtained Na-β"-Al2O3 powder, sodium source, zirconium source, silicon source, phosphorus source and carbon source are added to the solvent, dispersed, and then the positive electrode active material is added and dispersed to obtain a precursor slurry.
[0070] The obtained precursor slurry is calcined under a protective gas atmosphere after removing the solvent to obtain a surface-coated Na-β"-Al2O3, Na3Zr2Si2PO 12and a positive electrode active material of a carbon material, that is, a positive electrode material. In some embodiments, the aluminum source includes but is not limited to aluminum chloride, aluminum nitrate, aluminum sulfate, etc.; the sodium source used to prepare the Na-β"-Al2O3 block includes but is not limited to sodium chloride, sodium nitrate, sodium sulfate, etc.; the sodium source used to prepare the precursor slurry includes but is not limited to sodium acetate, sodium citrate, sodium carbonate, sodium bicarbonate, etc.; the zirconium source includes but is not limited to zirconium acetate, zirconium oxide, zirconium nitrate, zirconium oxynitrate, etc.; the silicon source includes but is not limited to silicon dioxide, ethyl silicate, sodium silicate, etc.; the phosphorus source includes but is not limited to phosphoric acid, ammonium hydrogen phosphate, sodium phosphate, sodium hydrogen phosphate, etc.; the carbon source used to prepare the Na-β"-Al2O3 block and the precursor slurry includes but is not limited to glucose, sucrose, starch, polyacrylonitrile, polyvinyl alcohol, polyvinyl pyrrolidone, polymethyl methacrylate, etc. In some embodiments, the solvent used to prepare the Na-β"-Al2O3 block and the solvent used to prepare the precursor slurry include but are not limited to water, ethanol, acetone, methanol, isopropanol, N-methylpyrrolidone, N,N-dimethylformamide, triethylene glycol, etc. In some embodiments, the calcination temperature for preparing the Na-β"-Al2O3 block is not less than 800°C, and the calcination time is greater than 1 hour. In some embodiments, the calcination temperature for preparing the precursor slurry is not less than 800°C, and the calcination time is greater than 1 hour.
[0071] (2) Secondary batteries / electrical equipment
[0072] According to a second aspect of the present application, a secondary battery or electrical device is provided, comprising a positive electrode plate, the positive electrode plate comprising a positive electrode collector and the above-mentioned positive electrode material, wherein the above-mentioned positive electrode material is distributed on at least one surface of the positive electrode collector.
[0073] The present application has no specific restrictions on the selection of the positive electrode current collector, and any positive electrode current collector of a secondary battery in the technical field can be selected.
[0074] In the present application, the secondary battery further comprises a negative electrode plate. The present application has no specific restrictions on the selection of the negative electrode plate, and any negative electrode plate of a secondary battery in the art can be selected.
[0075] In the present application, the secondary battery further comprises a separator. The present application has no specific restrictions on the selection of the separator, and any separator of a secondary battery in the art can be selected.
[0076] In the present application, the secondary battery also includes an electrolyte. The present application has no specific restrictions on the selection of the electrolyte, and any electrolyte of a secondary battery in the art can be selected.
[0077] This application has no specific restrictions on electrical equipment, such as electric vehicles.
[0078] The present application is further described below through specific examples.
[0079] Example 1
[0080] This embodiment provides a positive electrode material, including a positive electrode active material and a coating material, wherein the coating material is distributed on at least a portion of the surface of the positive electrode active material, and the coating material contains an electronic conductor and an ion conductor, wherein the positive electrode active material is an O3 phase NaN i0.33 Fe 0.33 Mn 0.33 O2, the electronic conductor is hard carbon, and the ion conductor is Na3Zr2Si2PO 12 ; The ratio of the particle size Dv50 of the positive electrode active material and the electronic conductor is 1:0.01, the ratio of the particle size Dv50 of the positive electrode active material and the ion conductor is 1:0.08, the particle size Dv10 of the ion conductor is 0.9μm, Dv50 is 2μm, Dv90 is 10μm, and Dv100 is 30μm; the mass of the ion conductor is 10% of the total mass of the electronic conductor and the ion conductor; the mass ratio of the ion conductor to the positive electrode active material is 1:500; the thickness of the coating material on the surface of the positive electrode active material is 8μm.
[0081] The preparation method of the positive electrode material of this embodiment includes the following steps: preparing 0.07g of ion conductor Na3Zr2Si2PO 12 The required precursors Na2CO3, ZrO(NO3)2, SiO2 and (NH4)2HPO4 were added to 50 mL of ethanol (wherein Na2CO3 was in excess of 2% to compensate for the volatilization of sodium during high temperature sintering), stirred evenly in a 60°C water bath, and then 0.98 g of polyvinyl pyrrolidone was added. Stirring was continued for 2 hours, and then 35.30 g of O3 layered oxide NaN with a Dv50 of 25 μm was added. i0.33 Fe 0.33 Mn 0.33 O2, stirred into a viscous slurry, and then transferred into an oven to be dried at 80°C to obtain a positive electrode precursor. The obtained positive electrode precursor was pre-fired at 230°C in a muffle furnace for 3 hours, cooled to room temperature, ground into a uniform powder, and then transferred into a tubular furnace and continuously introduced with high-purity argon gas. The temperature was raised to 950°C at 5°C / min and sintered for 2 hours, and then the temperature was lowered to room temperature to obtain an O3 layered oxide positive electrode material with dual ion and electron coating.
[0082] Example 2 to Example 3
[0083] A positive electrode material is provided, and its preparation method is the same as that of Example 1, except that the NaN i0.33 Fe 0.33 Mn 0.33 The particle size Dv50 of O2 is used to adjust the Dv50 ratio of the positive electrode active material to the electronic conductor and ion conductor.
[0084] Example 4 to Example 5
[0085] The preparation process of the positive electrode material is the same as that of Example 1, except that the heating rate is controlled to adjust the particle size and coating thickness of the generated ion conductor.
[0086] Example 6 to Example 9
[0087] The preparation process of the positive electrode material is the same as that of Example 1, except that the addition amounts of Na2CO3, ZrO(NO3)2, SiO2 and (NH4)2HPO4 are adjusted to adjust the content of the ion conductor in the coating material.
[0088] Example 10 to Example 15
[0089] The preparation process of the positive electrode material is basically the same as that of Example 1, except that Na3Zr2Si2PO 12 Replaced with other different ion conductors (see Table 1 for details).
[0090] Examples 16 to 18
[0091] The preparation process for the positive electrode material was the same as in the previous example, except that after heating to 950°C at 5°C / min for 2 hours and then cooling to room temperature, the powder was evenly dispersed in a PAN (polyacrylonitrile) solution and dried to obtain the positive electrode material. By adjusting the concentration of the PAN solution, positive electrode materials with different PAN mass contents were obtained.
[0092] Examples 19-20
[0093] The preparation process of the positive electrode material is the same as that of Example 1, except that NaNi 0.33 Fe 0.33 Mn 0.33 O2 is replaced by other positive electrode active materials.
[0094] Comparative Example 1 to Comparative Example 2
[0095] The preparation process of the positive electrode material is the same as that of the embodiment, except that the heating rate and the sintering temperature are adjusted to adjust the Dv50 ratio of the positive electrode active material to the electronic conductor and the Dv50 ratio of the positive electrode active material to the ion conductor.
[0096] Table 1
[0097] Among them, the first positive electrode active material in Table 1 represents O3 phase NaN i0.33 Fe 0.33 Mn 0.33 O2, the second positive electrode active material represents P2-O3 mixed phase Na 0.72 Ni 0.33 Fe 0.058 Mn0.532 Ti 0.08 O2, the third positive electrode active material represents Na3V2(PO4)3.
[0098] The positive electrode materials of each embodiment and comparative example were made into batteries, and the specific method was as follows:
[0099] The positive electrode material, conductive agent carbon black, and binder PVDF are mixed in a mass ratio of 90:5:5, and then an appropriate amount of NMP is added to stir into a slurry. The slurry is coated on one surface of a 16μm thick aluminum foil to obtain a positive electrode sheet. Then, it is assembled into a button-type battery with a negative electrode metal sodium sheet, a glass fiber separator, and an electrolyte (prepared by dissolving NaPF6 in a mixture of ethylene carbonate (EC) and propylene carbonate (PC), with a NaPF6 concentration of 1 mol / L and a volume ratio of EC and PC of 1:1).
[0100] The prepared battery was tested, wherein the test items are as follows:
[0101] 1) Normal temperature and low temperature rate performance test: The rate performance test was carried out at room temperature 25°C and low temperature -20°C respectively. The rate performance was tested using 0.5C, 2C, and 5C respectively, and the reversible capacity of the battery at different rates was recorded.
[0102] 2) Cycle performance test: At 25°C, place the battery aside for 5 minutes, charge it to 4.0V at a constant current rate of 1C, then charge it at a constant voltage until the current is less than or equal to 0.05C, then place it aside for 5 minutes, and then discharge it to 2.0V at a constant current rate of 1C. This is one charge and discharge cycle, and the discharge capacity this time is recorded as the discharge capacity of the first cycle of the lithium-ion secondary battery. The lithium-ion secondary battery is subjected to 200 cycle charge and discharge tests according to the above method, and the discharge capacity of each cycle and the last cycle is recorded. The capacity retention rate (%) of the battery after 200 cycles = discharge capacity of the 200th cycle / discharge capacity of the first cycle × 100%.
[0103] The test results are shown in Table 2.
[0104] Table 2
[0105] It can be seen from the above data that when the ratio of the particle size Dv50 of the positive electrode active material and the electronic conductor meets 1: (0.01~0.25), and the ratio of the particle size Dv50 of the positive electrode active material and the ion conductor meets 1: (0.08~0.5), the battery rate performance and cycle performance can be significantly improved.
[0106] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application and are not intended to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present application may be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present application.
Claims
1. A positive electrode material, in, The positive electrode material comprises a positive electrode active material and a coating material, wherein the coating material is distributed on at least a portion of the surface of the positive electrode active material; The coating material comprises an electronic conductor and an ion conductor; The ratio of the particle diameter Dv50 of the positive electrode active material and the electron conductor is 1:(0.01-0.25); and The ratio of the particle diameters Dv50 of the positive electrode active material and the ion conductor is 1:(0.08-0.5).
2. The positive electrode material according to claim 1, in, The particle size Dv50 of the ion conductor is 0.05 to 7.5 μm.
3. The positive electrode material according to claim 2, in, The particle size Dv50 of the ion conductor is 0.5 to 5 μm.
4. The positive electrode material according to claim 1, in, The ion conductor includes at least one of a first ion conductor and a second ion conductor, the first ion conductor having a Nasicon structure, and / or the second ion conductor having a layered structure.
5. The positive electrode material according to claim 4, in, The first ion conductor includes Na 3+Ax Zr 2-0.5Ax M x Si 2 PO 12 , wherein M is selected from at least one of Li, Ca, Mg, Sr, Ba, In, Ga, Nb, La, Cr, Mn, Zn, Al, Ge, and Bi, A is the valence state of the M element, and 0≤x≤0.5; and / or the second ion conductor includes Na y -β"-Al 2 O 3 , where 0 <y≤1。 6. The positive electrode material according to any one of claims 4 to 5, in, The mass ratio of the first ion conductor to the second ion conductor is 1:(0.16-6).
7. The positive electrode material according to any one of claims 1 to 5, in, The coating material further comprises a polymer, and the polymer comprises at least one of polyacrylonitrile, polyvinyl pyrrolidone and polyethylene oxide.
8. The positive electrode material according to claim 7, in, The mass of the polymer accounts for 0.5% to 3% of the total mass of the coating material.
9. The positive electrode material according to any one of claims 1 to 5, in, The mass of the ion conductor is 10% to 90% of the total mass of the electron conductor and the ion conductor.
10. The positive electrode material according to any one of claims 1 to 5, in, The coating material has a thickness of 0.6 to 8 μm on the surface of the positive electrode active material.
11. The positive electrode material according to any one of claims 1 to 5, in, The positive electrode active material includes at least one of a layered oxide and a polyanion positive electrode active material.
12. The positive electrode material according to any one of claims 1 to 5, in, The electron conductor includes a carbon material.
13. The positive electrode material according to any one of claims 1 to 5, in, The mass ratio of the ion conductor to the positive electrode active material is 1:(10-500).
14. A secondary battery, in, The secondary battery comprises the positive electrode material according to any one of claims 1 to 13.
15. An electrical device, in, The electrical device comprises the secondary battery according to claim 14, and the secondary battery serves as a power supply for the electrical device.
Citation Information
Patent Citations
Positive electrode body for nonaqueous electrolyte battery, method for producing same, and nonaqueous electrolyte battery
CN102893431A
Lithium ion battery anode material and preparation method thereof
CN103682356A
Positive electrode active material and high-voltage lithium ion battery comprising same
CN112542583A
Composite conductive paste, preparation method thereof, positive pole piece and lithium ion battery
CN113471412A
Positive electrode material, secondary battery and electric equipment
CN116364891A
Cited By
Composite sodium ion positive electrode material, preparation method thereof, positive plate and sodium ion battery
CN120164924A