Alkoxylated glycerol triacrylate, and use thereof and preparation method therefor

By developing low-functionalized alkoxylated glyceryl triacrylate and reacting the ring-opening oxetane oligomer with acrylic acid, the carcinogenicity problem of trimethylolpropane triacrylate and the ethoxylation problem in the existing technology are solved. It solves the problem of increased viscosity of trimethylol acrylate and achieves the effects of excellent flexibility and moderate viscosity, and is suitable for a variety of photocurable materials.

WO2024199017A1PCT designated stage expired Publication Date: 2024-10-03CHANGZHOU TRONLY NEW ELECTRONICS MATERIALS CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/082520
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The existing trimethylolpropane triacrylate is prohibited from being used in cosmetics production due to its carcinogenicity, and its substitute, ethoxylated trimethylolpropane triacrylate, increases in viscosity when increasing flexibility, affecting its use and making it difficult to find the viscosity. Excellent alternative for moderate flexibility.

Method used

Develop a low-functionalized alkoxylated glyceryl triacrylate, whose structure regulates viscosity through specific group chain length, and is prepared by the reaction of oxetane oligomer ring opening and acrylic acid, using strong protonic acid and phase The transfer catalyst controls the reaction, and the preparation process is simple and the cost is low.

Benefits of technology

The prepared alkoxylated glyceryl triacrylate exhibits excellent flexibility and moderate viscosity in photo-curable materials, is suitable for a variety of photo-cured materials, and has a safe process and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024082520_03102024_PF_FP_ABST
    Figure CN2024082520_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Alkoxylated glycerol triacrylate, and the use thereof and a preparation method therefor. The alkoxylated glycerol triacrylate is represented by a structure as shown in formula (I). The preparation method for the alkoxylated glycerol triacrylate has a simple process and relatively low production cost; moreover, the prepared alkoxylated glycerol triacrylate has a moderate viscosity, and a formed photocuring composition containing same has relatively high curing sensitivity and good flexibility.
Need to check novelty before this filing date? Find Prior Art

Description

Alkoxylated glycerol triacrylate, its application and preparation method

[0001] This application claims the benefit of Chinese patent application No. 2023103110619, filed on March 28, 2023. This application incorporates the entire text of the aforementioned Chinese patent application. Technical Field

[0002] The present application relates to the field of photocuring, and in particular to an alkoxylated glycerol triacrylate, and its application and preparation method. Background Art

[0003] Trimethylolpropane triacrylate (TMPTA) is a typical trifunctional monomer. Its viscosity is higher than that of monofunctional and difunctional monomers, but lower than that of multifunctional monomers, resulting in excellent solvency. This monomer offers a high cure speed and high crosslink density, forming a hard, scratch-resistant, but brittle cured film with excellent solvent resistance. Although it is relatively inexpensive and somewhat irritating to the skin, it remains the most commonly used multifunctional monomer. However, due to its known carcinogenicity, TMPTA is banned from use in cosmetics, necessitating the search for new alternatives.

[0004] Ethoxylated trimethylolpropane triacrylate is one of its substitutes. Introducing ethoxy groups into multifunctional monomer molecules can increase the flexibility of the molecules. As the ethoxy content increases, the flexibility of the molecules increases, but its viscosity increases, affecting its use.

[0005] Comparative documents: CN102503821A, CN100480301A, CN1298694A, CN102503821A, CN105439852B.

[0006] Summary of the Invention

[0007] The main purpose of the present application is to provide a low-functionalized alkoxylated glycerol triacrylate, its application and preparation method, which has excellent flexibility and moderate viscosity and can be well used in photocurable materials.

[0008] In order to achieve the above-mentioned purpose, the alkoxylated glycerol triacrylate of the present application has a structure as shown in the following formula (I):

[0009] Wherein, R1 and R2 are each independently methyl or hydrogen, and n≥1. The short chain length of the above groups can make the viscosity of the alkoxylated glycerol triacrylate moderate, which is beneficial for improving flexibility; and the synthetic raw materials are readily available and low in cost.

[0010] Another aspect of the present application is the use of the above-mentioned alkoxylated glyceryl triacrylate in photocurable materials, which include: one or more of: coatings, protective film materials, adhesives, photodegradable coatings, coatings, molded objects, optical recording media, 3D printing inks, interlayer insulating films, light extraction films, brightness enhancement films, printing inks, or photocurable inks for inkjet printing.

[0011] Another aspect of the present application is a method for preparing the above-mentioned alkoxylated glycerol triacrylate, comprising the following steps:

[0012] (1) epoxy ring opening of oxetane oligomer to obtain polyhydroxy compound;

[0013] (2) The polyhydroxy compound further reacts with acrylic acid to obtain the target product.

[0014] Furthermore, a strong proton acid is added to the ring-opening reaction of step (1) for ring-opening. The strong proton acid is one or more of methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, dodecylsulfonic acid, sulfuric acid, hydrochloric acid, or sulfonic acid; preferably, the strong proton acid is methanesulfonic acid or p-toluenesulfonic acid. The strong proton acid has strong acidity and a controllable ring-opening rate, making it easier to separate by-products, thereby facilitating the acquisition of the target intermediate.

[0015] Furthermore, a reaction solvent is added to the ring-opening reaction in the above step (1), and the reaction solvent is any one of water, a phase transfer catalyst or an organic solvent; the phase transfer catalyst is one or more of a cyclic crown ether, a quaternary phosphonium salt or a quaternary ammonium salt, preferably a quaternary ammonium salt.

[0016] Furthermore, the ring-opening reaction temperature in step (1) is 50-150° C.; preferably, the ring-opening reaction temperature in step (1) is 100° C.; and / or the ring-opening reaction time in step (1) is 4 hours. When the ring-opening reaction temperature is too low or the time is too short, the ring-opening reaction is difficult to proceed; when the ring-opening reaction temperature is too high, the reaction will be too violent, and since the ring-opening reaction is an exothermic reaction, too high a temperature will easily cause danger during testing and production.

[0017] Furthermore, the temperature of step (2) is 50-150°C; preferably, the reaction temperature of step (2) is 110°C; and / or the reaction time of step (2) is 3 hours. If the reaction temperature is too low or the reaction time is too short, the reaction will be too slow; if the reaction temperature is too high, the material will easily aggregate violently, affecting production safety.

[0018] Furthermore, in the above step (2), a reaction solvent is added, and the reaction solvent is one or more of toluene, benzene, cyclohexane, n-heptane, cyclopentane, isopropyl ether, methyl tert-butyl ether or ethylene glycol monomethyl ether.

[0019] Furthermore, a polymerization inhibitor is added in the above step (2); preferably, the polymerization inhibitor is tetrabutylammonium bromide. The above polymerization inhibitor can better control the reaction process and is conducive to obtaining the target product.

[0020] The preparation method of the alkoxylated glycerol triacrylate is simple in process and low in production cost. The prepared alkoxylated glycerol triacrylate has moderate viscosity, and the photocurable composition formed therefrom has high curing sensitivity and excellent flexibility. DETAILED DESCRIPTION

[0021] Example 1

[0022] 1. Synthesis of Intermediate 1a

[0023] 27.3 g of raw material 1a (weight average molecular weight of 273) and 1.6 g of methanesulfonic acid were dissolved in 30 mL of deionized water, heated to 100° C. and refluxed for 4 h to obtain intermediate 1a.

[0024] 2. Synthesis of Compound 1a

[0025] The intermediate 1a obtained in the previous reaction, 8.6 g of acrylic acid, and 50 mL of toluene were added to a 250 mL four-necked flask. The resulting solution was heated at 110°C and refluxed for 3 h while removing the generated water. The acid value of the reaction system was monitored until it no longer changed. The solution was cooled to room temperature and distilled under reduced pressure to obtain 34.2 g of compound 1a.

[0026] Examples 2-7

[0027] Example 2: Referring to Example 1, the reaction raw material 1a was replaced with 2a (weight average molecular weight of 321) to obtain compound 2a;

[0028] Example 3: Referring to Example 1, the reaction raw material 1a was replaced with 3a (weight average molecular weight of 389) to obtain compound 3a;

[0029] Example 4: Referring to Example 1, the reaction raw material 1a was changed to 4a ( The weight average molecular weight is 289) to obtain compound 4a;

[0030] Example 5: Referring to Example 1, the reaction raw material 1a was changed to 5a ( The weight average molecular weight is 439) to obtain compound 5a;

[0031] Example 6: Referring to Example 1, the catalyst was replaced with p-toluenesulfonic acid to obtain compound 2a;

[0032] Example 7: Referring to Example 1, the first step reaction solvent was changed to 30 mL of toluene, and 0.2 g of tetrabutylammonium bromide was added to obtain compound 2a;

[0033] Furthermore, the present application also includes the use of the above-mentioned compounds in photocurable materials. By formulating exemplary radiation-curable compositions, the application performance of the alkoxylated glyceryl triacrylate of the present application is evaluated.

[0034] A radiation-curable composition was prepared by selecting a common initiator, the monomers described herein, and a common acrylate monomer for comparison according to Table 1. The weight percent (wt %) is based on the total weight of the radiation-curable composition. The composition is as follows:

[0035] Table 1

[0036] Compound A: trimethylolpropane triacrylate; Compound B: 6(ethoxy)trimethylolpropane triacrylate, T063

[0037] The photocurable composition was stirred and mixed under a yellow light lamp, and the material was rolled onto a PET template to form a film with a thickness of about 20 μm. The film was exposed by a crawler type method and irradiated with a high-pressure mercury lamp (exposure machine model RW-UV70201, wavelength 200-500 nm, light intensity 226 mW / cm2), and the curing condition of the cured film was observed.

[0038] (1) Curing sensitivity

[0039] The curing sensitivity of the monomer was evaluated by finger touch method: A: dry surface; B: slightly sticky after curing; C: uncured;

[0040] (2) Flexibility evaluation method: bending test

[0041] Referring to the paint film flexibility test standard GB / T 1731-93, the outer side of the tinplate coated with the cured coating was wound along the length direction on rods with diameters of 10, 5, 4, 3, 2, and 1 mm in sequence, bent for 2-3 seconds, and observed with a magnifying glass. The flexibility of the UV-cured coating was indicated by the diameter of the rod that caused the smallest damage to the coating layer.

[0042] The test results are shown in Table 2.

[0043] Table 2

[0044] In summary, the alkylated glycerol triacrylate described in the present application can not only be cured well, but also has excellent flexibility after curing.

Claims

1. An alkoxylated glyceryl triacrylate, characterized in that: The structure represented by the following formula (I): Wherein, R1 and R2 are each independently methyl or hydrogen, and n≥1.

2. Use of the alkoxylated glycerol triacrylate according to claim 1 in a photocurable material, wherein the photocurable material comprises: One or more of coatings, protective film materials, adhesives, photodegradable coatings, coatings, molded products, optical recording media, 3D printing inks, interlayer insulating films, light extraction films, brightness enhancement films, printing inks, or photocurable inks for inkjet printing.

3. A method for preparing alkoxylated glycerol triacrylate according to claim 1, characterized in that: As shown in the following formula, the specific steps include: (1) epoxy ring-opening of oxetane oligomer to obtain polyhydroxy compound; (2) The polyhydroxy compound is further reacted with acrylic acid to obtain the target product.

4. The method for preparing alkoxylated glycerol triacrylate as claimed in claim 3, characterized in that: In the ring-opening reaction described in step (1), a strong proton acid is added to open the ring.

5. The method for preparing alkoxylated glycerol triacrylate as claimed in claim 4, characterized in that: The strong protonic acid in the above step (1) is any one or more of methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, dodecylsulfonic acid, sulfuric acid, hydrochloric acid or sulfonic acid; preferably, the strong protonic acid is methanesulfonic acid or p-toluenesulfonic acid.

6. The method for preparing alkoxylated glycerol triacrylate as claimed in claim 3, characterized in that: In the above step (1), a reaction solvent is added, and the reaction solvent is any one of water, a phase transfer catalyst or an organic solvent.

7. The method for preparing alkoxylated glycerol triacrylate as claimed in claim 3, characterized in that: The ring-opening reaction temperature in the above step (1) is 50-150°C; preferably, the ring-opening reaction temperature in the above step (1) is 100°C; and / or the ring-opening reaction time in the above step (1) is 4h.

8. The method for preparing alkoxylated glycerol triacrylate as claimed in claim 3, characterized in that: The reaction temperature in step (2) is 50-150°C; preferably, the reaction temperature in step (2) is 110°C; and / or the reaction time in step (2) is 3h.

9. The method for preparing alkoxylated glycerol triacrylate as claimed in claim 3, characterized in that: In the above step (2), a reaction solvent is added, and the reaction solvent is one or more of toluene, benzene, cyclohexane, n-heptane, cyclopentane, isopropyl ether, methyl tert-butyl ether or ethylene glycol monomethyl ether.

10. The method for preparing alkoxylated glycerol triacrylate as claimed in claim 3, characterized in that: In the above step (2), a polymerization inhibitor is added; preferably, the polymerization inhibitor is tetrabutylammonium bromide.

Citation Information

Patent Citations

  • Method for producing triacrylic ester of alkoxylating trimethylolpropane

    CN101092354A

  • Method for preparing ethoxylation <15> trimethylol propyl triacrylate

    CN102146036A

  • Preparation method of ethoxylated trimethylolpropane triacrylic ester

    CN102173989A

  • Clean production method of alkoxylation glycerol triacrylate

    CN102503821A

  • Curable resin composition and molded article produced by utilizing said composition

    JP1987007711A