Paper with transparency properties, device and method for applying the properties thereto

By infusing cellulose paper with a food-safe wax and triglycerides and applying a specific treatment process, the paper achieves transparency and humidity control, addressing the limitations of existing packaging materials and offering an environmentally friendly, recyclable solution for packaging fresh products.

WO2024200885A1PCT designated stage expired Publication Date: 2024-10-03PLASTICOS DEL SEGURA SL
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/ES2023/070335
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2023-05-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current packaging materials, such as plastic and paper, fail to balance breathability and transparency, leading to issues like moisture retention or loss, and environmental concerns, with existing solutions relying on composite materials that excessively use plastic.

Method used

A sheet of paper with cellulose fibers, a Cobb absorption index greater than 28 g/m², porosity greater than 300 ml/cm², and humidity between 3-7%, infused with a food-safe wax and triglycerides, is treated using equipment with infrared heating and a component application process to achieve transparency without adding plastic.

Benefits of technology

The resulting paper is 100% recyclable, provides transparent optical properties for product visibility, maintains humidity control, and is suitable for food packaging without the environmental drawbacks of plastic, ensuring the product's quality and appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure ES2023070335_03102024_PF_FP_ABST
    Figure ES2023070335_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to paper with transparency properties, a device and a method for applying the properties thereto, wherein the paper comprises a sheet of paper and a component including a wax and an additive formed by triglycerides that is integrated between cellulose fibres. The device comprises an inlet surface with heating means, a first roller, a gun for applying the component, one or more knurling cylinders, a calender with at least two second rollers, and a third roller with cooling means. The method begins with heating the sheet on the inlet surface, followed by moving the sheet between the first roller and the gun, injecting the component by means of the gun and applying pressure by means of the knurling cylinder, then moving the sheet by means of the second rollers and the third cooled roller, and lastly removing the sheet.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] DESCRIPTION

[0002] Paper with transparency properties, equipment and procedure for applying said properties to it

[0003] Technical field of the invention

[0004] The present invention corresponds to the technical field of coating or packaging materials used to wrap products or to manufacture containers in which to contain them.

[0005] Background of the Invention

[0006] Nowadays, most products are packaged in one way or another. For non-fresh products, this packaging is usually more elaborate, but for fresh products, simpler packaging is used, such as a plastic bag or a paper bag, which allows for transport while protecting the product inside and maintaining its properties.

[0007] In the case of plastic bags or wrappers, in addition to the negative impact they have on the environment, we must consider the disadvantages they pose for certain products, as they fail to preserve the qualities of the product being preserved.

[0008] Paper, on the other hand, has multiple advantages: it is biodegradable, reusable, and, because it is breathable, it naturally eliminates microorganisms through contact with oxygen.

[0009] Plastic is an impermeable material that doesn't allow the product inside to breathe, so the moisture inside is trapped, making it gummy and unattractive. Furthermore, it isn't temperature-resistant, making it unsuitable for certain products that are hot-packed. Paper, on the other hand, is breathable, but this can cause the product to lose moisture too quickly and dry out. To solve this problem, current technology is focused on finding ways to achieve controlled, regulated breathability of the paper by applying a level of waterproofing that allows some of the product's moisture to be retained, just the right amount.

[0010] However, there is another characteristic that differentiates plastic and paper, which is not being taken into consideration: plastic can have a quality, that of transparency, that paper does not have.

[0011] This is a problem because it's important for consumers to be able to see the product inside the packaging to appreciate its characteristics. This applies to bags or any other type of packaging, as when made of plastic they are transparent, but when made of paper this is not possible.

[0012] In the state of the art, there are some ways to solve this problem by creating visibility spaces or windows, formed by portions of transparent plastic material, which are added to the paper, using adhesives or other joining means, and thus allowing the interior of the bag to be visible through this window.

[0013] As an example of the state of the art, reference document ES2271096 can be mentioned.

[0014] This document, ES2271096, defines a bag for wrapping food products, especially bread, rolls, and snacks, made of a composite material with at least a first layer of cellulose material and a second layer of plastic. Furthermore, the composite material is perforated, and the first layer of cellulose material is interrupted in at least one area to create a viewing window.

[0015] This solution aims to control the bag's breathability by using two layers, one of paper and the other of plastic, with common holes. It also aims to solve the problem of transparency, allowing the product inside to be viewed.

[0016] However, the main problem, the excessive use of plastic and the harm it causes to our environment, is not being considered.

[0017] In other cases, the procedures the paper undergoes focus on applying a coating to one side of the paper, attempting to reduce its permeability to levels suitable for good product preservation. However, they still do not address the issue of the transparency required by these materials to properly perform their packaging functions.

[0018] It is therefore necessary to find a way to solve this problem, by obtaining a packaging material that is transparent and does not involve the use of plastics.

[0019] Description of the invention

[0020] The paper with transparency properties presented here comprises a paper sheet formed by cellulose fibers that has a Cobb absorption index whose value is greater than 28 gr / m 2 , a porosity with a value greater than 300 ml / cm 2, and a humidity between 3 and 7%.

[0021] In addition, this paper contains a component consisting of a food-safe wax and an additive consisting of triglycerides in a proportion of between 5 and 10% of the total weight of the component.

[0022] This component is absorbed by the paper sheet, such that it becomes embedded between the cellulose fibers. Also presented is a device for applying transparency properties to a paper as defined above, which comprises an input surface with infrared heating means.

[0023] This equipment also features a first hot roller located below the infeed surface and a component application gun. This gun is located above the first roller, so that the two create a space between them that allows the paper sheet to pass through.

[0024] The gun is connected to an injection pump and comprises a rod of width equal to or greater than the width of the sheet, connected to a rotating motor.

[0025] This equipment also has one or more knurled cylinders coaxially connected to the rod and a calender formed by at least two second hot rollers arranged after the passage space, where both second rollers have a diameter such that the paper travels over them is greater than or equal to 3 m.

[0026] Finally, it features a third double roller with cooling means at a second temperature.

[0027] A procedure is also proposed for applying transparency properties to paper using equipment such as those previously defined.

[0028] This process comprises a first phase consisting of a sheet of paper being applied to the input surface at a given speed.

[0029] The second phase consists of heating the paper sheet to a first determined temperature, simultaneously with its movement over the input surface.

[0030] Next, a third phase of moving said sheet of paper through the passage space between the first roller and the component application gun is carried out, where the gun rod rotation motor has a tangential speed equal to the speed of movement of the sheet.

[0031] The fourth phase consists of injecting the component using the gun onto the knurled cylinder, at a specific flow rate and temperature, simultaneously with the movement of the sheet through the passage space.

[0032] Simultaneously with the rotation of the rod and the injection of the component, a fifth phase of applying pressure to the surface of the paper sheet takes place, by means of the knurled cylinder, such that it is capable of allowing the penetration of the component between the fibers of the sheet in a width of the sheet equal to or less than that of the knurled cylinder.

[0033] A sixth phase is then carried out, moving the paper sheet along a length greater than or equal to 3 m through the calender with two second hot rollers, where these second rollers have a tangential speed equal to the speed of movement of the paper sheet.

[0034] Finally, a seventh phase of displacement of the paper sheet over a third double roller which has a second temperature for cooling, and an eighth phase of removal of the sheet takes place.

[0035] The paper with transparency properties proposed here represents a significant improvement in the state of the art.

[0036] This is because a material is obtained whose optical properties can be modified, either in a specific area or in its entirety.

[0037] This material is not intended to provide waterproofing or visual appeal through a glossy or satiny optical effect, but rather to provide transparency that allows the product inside to be distinguished once packaged in this material. This material, with the integrated component inside, is suitable for food use and can be used in the production of bags, containers, container lids, and so on.

[0038] Furthermore, this component can be applied to the entire paper sheet, to a strip of paper, or to separate areas of the sheet, depending on the desired application and the intended use of the sheet. For example, in the case of bags for transporting loaves of bread, a longitudinal strip can be applied to the paper sheet, allowing perfect visual access to the inside of the bag.

[0039] It is a completely recyclable material, as transparency is achieved without any added plastic. No other material is added either, as the structural composition of all or part of the sheet is altered. However, it remains a sheet without any attached pieces or materials, making it more resistant and avoiding the problem of separation or breakage of the bonds between materials.

[0040] Furthermore, since the component is integrated into the paper's interior, between its fibers, it does not result in an oily finish, as it is not applied superficially but at the structural level.

[0041] The procedure applied with the appropriate equipment allows the component to penetrate between the fibers of the paper sheet, achieving integration of the component into the paper and not a coating on one side of it.

[0042] It is therefore a very effective paper that offers transparency properties without the use of plastics or derivatives, making it 100% recyclable.

[0043] Brief description of the drawings

[0044] In order to assist in a better understanding of the characteristics of the invention, according to a preferred example of practical embodiment thereof, a series of drawings are provided as an integral part of said description, where, for illustrative and non-limiting purposes, the following has been represented:

[0045] Figure 1.- Shows a perspective view of the equipment for applying transparency properties to a paper, for a first preferred embodiment of the invention.

[0046] Figure 2.- Shows a profile view of the equipment for applying transparency properties to a paper, for a first preferred embodiment of the invention.

[0047] Figure 3.- Shows a perspective view of a paper with transparency properties obtained by the equipment, for a first preferred embodiment of the invention.

[0048] Figure 4.- Shows a perspective view of a paper with transparency properties obtained by the equipment, for a second preferred embodiment of the invention.

[0049] Detailed description of a preferred embodiment of the invention

[0050] In view of the figures provided, it can be seen how in a first preferred embodiment of the invention, the paper with transparency properties, which is proposed here, comprises a sheet (1) of paper formed by cellulose fibers that has a Cobb absorption index whose value is greater than 28 gr / m 2 , a porosity with a value greater than 300 ml / cm 2 , and a humidity between 3 and 7%.

[0051] In addition, it comprises a component consisting of a food-safe wax and an additive consisting of triglycerides in a proportion between 5 and 10% of the total weight of the component.

[0052] This component is absorbed by the paper sheet (1) such that it is integrated between the cellulose fibers, therefore, a compound is sought that has a high power of penetration into the paper sheet. Therefore, a paper sheet (1) with a high absorption capacity is sought that is capable of absorbing the component in its structure. Until now, in the paper sheets with which we worked, the opposite was sought, that is, an absorption capacity as low as possible, because, the greater the absorption capacity, the more water the fibers have and this makes them less resistant and, in addition, greater absorption generates a greater consumption of products from the final paper finishing, such as glues, inks...

[0053] In the case of this invention and the objective pursued, it must be taken into account that the transparency of the paper is achieved when the light rays pass through the labyrinth of fibers and air that make up the paper sheet and manage to exit it.

[0054] The structure of paper fiber is formed by an amalgamation of cellulose fibers of different sizes, bleaching agents, sizing agents, and fillers. Therefore, the objective sought in this invention is to ensure that light can pass through this structure as easily as possible. This is achieved by reducing the difference between the refractive index of the cellulose fibers and the air surrounding them. If the spaces between the fibers, occupied by air, are filled with a component with a refractive index more similar to that of cellulose than that of air, the desired objective is achieved.

[0055] The absorption rate of cellulose paper depends on three factors: the Cobb index, a parameter used to measure the paper's ability to absorb water or any other type of liquid; porosity, which is the ratio of the volume occupied by air to the total volume of paper; and humidity.

[0056] Humidity is directly related to the ability to absorb other elements. Lower humidity means greater capacity and a higher Cobb index.

[0057] Thus, depending on these variables, different transparency results are obtained. In this first preferred embodiment of the invention, the paper sheet (1) has a weight of 32 g / m 2 and the Cobb absorption index has a value greater than 28 gr / m 2 and the porosity has a value greater than 300 ml / cm 2 .

[0058] In another embodiment, the sheet (1) of paper has a weight of 35 gr / m 2 and the Cobb absorption index has a value greater than 32 gr / m 2 and the porosity has a value greater than 350 ml / cm 2 .

[0059] Furthermore, in another preferred embodiment, the paper sheet (1) has a weight of 40 gr / m 2 and the Cobb absorption index has a value greater than 35 gr / m 2 and the porosity has a value greater than 400 ml / cm 2 .

[0060] As already indicated, on the one hand, the paper sheet (1) must be as absorbent as possible in order to fill the gaps with a component that must have a refractive index that is as similar as possible to the refractive index of cellulose.

[0061] In this first preferred embodiment of the invention, the component comprises a wax formed from at least one vegetable wax. In other embodiments, the wax is formed from at least one paraffin.

[0062] Furthermore, in this first preferred embodiment, the triglycerides are formed by a mixture of palmitic acid and linoleic acid.

[0063] Vegetable waxes are used in the component, but from a thermodynamic point of view, they have no affinity with the cellulose in paper. For this reason, an additive such as the aforementioned vegetable oils is used.

[0064] The goal is to convert the polarity of cellulose into apolarity, thereby creating affinity with the vegetable wax. This is achieved by mixing vegetable wax with triglycerides. These long-chain triglycerides, such as palmitic acid and linoleic acid, convert the vegetable wax into apolarity, thereby facilitating the creation of bonds between cellulose and vegetable wax.

[0065] In this first preferred embodiment of the invention, the transparency properties are in at least one area of ​​the paper sheet, which in this case is a band (2) of the sheet (1), as shown in Figure 2. In other preferred embodiments, the transparency properties are in the entire paper sheet (1).

[0066] It can also occur as shown in Figure 3, which represents the result obtained with a paper in which the transparency properties are in several areas of the sheet (1) of paper, which can be two or more continuous bands, or as in this second preferred embodiment, two discontinuous bands (2), that is, formed by aligned and separated portions from each other.

[0067] This document also proposes equipment for applying transparency properties to paper as previously defined.

[0068] As shown in Figures 1 and 2, this equipment comprises an input surface (3) that has heating means (4) using infrared.

[0069] It also has a first hot roller (5) located after the input surface (3) and a gun (6) for applying the component.

[0070] This gun (6) is located on the first roller (5), such that between them they form a space capable of allowing the passage of the paper sheet (1). The gun (6) is connected to an injection pump and has an inlet (6.1) for the component from the pump. It also comprises a rod (7) of a width equal to or greater than the width of the sheet (1), connected to a rotation motor (not shown in the Figures).

[0071] The equipment has one or more knurled cylinders (8) coaxially connected to the rod (7). In the first proposed embodiment, as shown in Figure 3, it comprises a knurled cylinder (8), to generate a band (2) with transparency properties in the sheet (1), while, as can be seen in Figure 4, in a second embodiment, the equipment has two knurled cylinders (8) and with them two bands (2) with transparency properties are obtained, which in this case are discontinuous, but in other cases they can be continuous.

[0072] As shown in Figures 1 to 3, the equipment also comprises a calender formed by at least two second hot rollers (9) arranged after the passage space (11), and a third double roller (10) arranged after the calender, which has cooling means at a second temperature.

[0073] In this first preferred embodiment of the invention, the gun (6) comprises a reducing element for its application nozzle.

[0074] Likewise, in this first embodiment, the gun (6) comprises an encoder for applying the component in pulses in a discontinuous manner when necessary. With an encoder, a sheet (1) can be obtained as shown in Figure 4, for a second embodiment, with discontinuous bands (2).

[0075] Likewise, in this case the gun (6) comprises a photocell.

[0076] This report also presents a procedure for applying transparency properties to a paper as defined and with the equipment described above.

[0077] This procedure comprises a first phase consisting of a sheet (1) of paper being fed onto the input surface (3) at a given speed.

[0078] A second phase consists of heating the paper sheet (1) to a first determined temperature, simultaneously with its movement over the input surface (3). In this first preferred embodiment of the invention, the first application temperature of the component is between 100 and 110°. With this heating of the paper sheet (1) its humidity is reduced to an amount of 5%.

[0079] The third phase consists of a displacement of the paper sheet (1) through the space (11) between the first roller (5) and the component application gun (6). The rod rotation motor (7) has a tangential speed equal to the speed of displacement of the sheet (1).

[0080] Next, a fourth phase of injection of the component takes place by means of the gun (6) on one or more knurled cylinders (8), with a determined flow rate and temperature, simultaneously with the movement of the sheet (1) through the passage space (11).

[0081] In this first preferred embodiment of the invention, the component application temperature is equal to the first temperature. In this way, the existence of thermal shock between the paper sheet (1) and the component is avoided at the time it is deposited on it and, therefore, the liquid phase of the component is not interrupted, facilitating its penetration into the structure of the paper sheet (1).

[0082] The fifth phase consists of applying pressure to the surface of the paper sheet (1) by means of the knurled cylinder (8) simultaneously with the rotation of the rod (7) and the injection of the component, such that it is capable of allowing the penetration of the component between the fibers of the sheet (1) in a width equal to or less than that of the knurled cylinder (8).

[0083] The knurling of the cylinder is what actually introduces and brings the component into contact with the sheet (1) of paper. This knurling must have sufficient capacity to prevent the application band (2) from opening. The knurling of the rod (7) varies depending on the component input required, so that the higher the paper grammage, the greater the input requirement. This knurling also depends on another factor, such as the working speed.

[0084] Thus, the higher the working speed, the greater the opening of the engraved cell required for knurling. In this first preferred embodiment of the invention, the travel speed of the paper sheet (1) is 40 m / min and knurling with a 120° opening cut is sufficient for the component to completely emerge from the cell.

[0085] In other embodiments with speeds of 60 m / min, a 130° cell opening is required, while for speeds of 100 m / min, the cell opening must be 140°.

[0086] The knurled cylinder (8) receives the component delivered by the nozzle of the gun (6) and deposits it under pressure on the sheet (1) of paper, pressing against the first roller (5), which in this first embodiment is formed by a high-hardness rubber roller. In this way, the component penetrates under pressure into the interior of the sheet (1) of paper.

[0087] As already indicated, the speed of the rod (7) and the paper sheet (1) is the same. This ensures that the component applied to the knurled cylinder (8) is transferred to the paper without any drag or build-up.

[0088] The rod (7) is connected to a motor that provides it with rotational motion. This motor is connected to a variable speed drive that receives information on the material flow rate from the same tachometer as the drive pump.

[0089] In this way we ensure that the nozzle of the rod (7) is synchronized to the speed of the paper, as is the drive pump. Both the pump mechanism and the rod receive the information of the speed of passage of the sheet (1) of paper from the same tachometer and both have to be perfectly synchronized. The sixth phase of this procedure consists of a displacement of the sheet of paper (1) for a time greater than or equal to 3 minutes, through the calender, where the second rollers (9) have a tangential speed equal to the speed of displacement of the sheet (1) of paper.

[0090] This minimum time of 3 min at high temperature allows the component to fully penetrate the structure of the paper sheet (1).

[0091] A seventh phase consists of moving the paper sheet (1) over a third double roller (10) which has a second cooling temperature. This temperature drop causes the component to cool inside the structure of the paper sheet (1), thus becoming integrated into it.

[0092] Finally, an eighth and final phase consists of removing the sheet (1).

[0093] In this first preferred embodiment of the invention, as shown in Figure 3, the application of the component is carried out in a band (2) on the sheet (1) of paper and this band (2) has a width equal to the width of a reducing element of the application nozzle of the gun (6).

[0094] In a second preferred embodiment, the component is applied discontinuously to the sheet (1) of paper according to the pulses generated by an encoder of the gun (6), as can be seen in Figure 4.

[0095] In other preferred embodiments of the invention, the sheet (1) of paper comprises at least one print on its surface and the injection of the component onto the knurled cylinder (8) comprises an initial reading step by means of a photocell of the gun (6) connected to the pump to determine the existence or absence of printing on the sheet (1) such that the pump is capable of stopping the injection of the gun (6) when it detects a print and activating the same when it detects the absence of printing.

Claims

CLAIMS 1- Paper with transparency properties, characterized in that it comprises a sheet (1) of paper formed by cellulose fibers that has a Cobb absorption index whose value is greater than 28 gr / m 2 , a porosity with a value greater than 300 ml / cm 2 , and a humidity between 3 and 7% and, a component comprising a wax suitable for food use and an additive formed by triglycerides in a proportion between 5 and 10% with respect to the total weight of the component, where this component is absorbed by the paper sheet, such that it is integrated between the cellulose fibers. 2- Paper according to claim 1, wherein the wax is formed by at least one vegetable wax. 3- Paper according to claim 1, wherein the wax is formed by at least one paraffin. 4- Paper according to any of the preceding claims, wherein the triglycerides are formed by a mixture of palmitic acid and linoleic acid. 5- Paper according to any of the preceding claims, wherein the sheet (1) of paper has a weight of 32 gr / m 2 and the Cobb absorption index has a value greater than 28 gr / m 2 and the porosity has a value greater than 300 ml / cm 2 . 6- Paper according to any of claims 1 to 4, wherein the sheet (1) of paper has a weight of 35 gr / m 2 and the Cobb absorption index has a value greater than 32 gr / m 2 and the porosity has a value greater than 350 ml / cm 2 . 7- Paper according to any of claims 1 to 4, wherein the sheet (1) of paper has a weight of 40 gr / m 2 and the Cobb absorption index has a value greater than 35 gr / m 2and the porosity has a value greater than 400 ml / cm 2 . 8- Paper according to any of the preceding claims, wherein the transparency properties are in at least one area of ​​the paper sheet (1). 9- Equipment for applying transparency properties to a paper, as defined in claims 1 to 8, characterized in that it comprises - an input surface (3) having heating means (4) by means of infrared; - a first hot roller (5) located after the inlet surface (3); - a gun (6) for applying the component located on the first roller (5), such that between the two they form a space (11) capable of allowing the passage of the sheet (1) of paper, where the gun (6) is connected to an injection pump and comprises a rod (7) of a width equal to or greater than the width of the sheet (1), connected to a rotation motor; - one or more knurled cylinders (8) coaxially connected to the rod (7); - a calender formed by at least two second hot rollers (9) arranged after the passage space (11), where both second rollers (9) have a diameter such that the paper travel on them is greater than or equal to 3 m, and; - a third double roller (10) arranged after the calender, which has cooling means at a second temperature. 10- Equipment according to claim 9, wherein the gun (6) has a reducing element of its application nozzle. 11- Equipment according to any of claims 9 or 10, wherein the gun (6) comprises an encoder for applying the component by means of discontinuous pulses. 12- Equipment according to any of claims 9 to 11, wherein the gun (6) comprises a photocell. 13- Procedure for applying transparency properties to a paper as defined in claims 1 to 8, by means of equipment as defined in claims 9 to 12, characterized in that it comprises - a contribution of a sheet (1) of paper onto the input surface (3) at a given speed; - heating the sheet (1) of paper to a first determined temperature, simultaneously with its movement on the input surface (3); - a movement of said sheet (1) of paper through the passage space (11) between the first roller (5) and the gun (6) for applying the component, where the rotation motor of the rod (7) of the gun has a tangential speed equal to the speed of movement of the sheet (1); - an injection of the component by means of the gun (6) onto one or more knurled cylinders (8), with a determined flow rate and temperature, simultaneously with the movement of the sheet (1) through the passage space (11); - an application of pressure on the surface of the sheet (1) of paper, by means of the knurled cylinder (8) simultaneously with the rotation of the rod (7) and the injection of the component, such that it is capable of allowing the penetration of the component between the fibers of the sheet (1) in a width equal to or less than that of the knurled cylinder (8); - a displacement of the sheet (1) of paper along a length greater than or equal to 3 m through the calender with two second rollers (9), where these second rollers (9) have a tangential speed equal to the speed of displacement of the sheet (1) of paper; - a displacement of the sheet (1) of paper on a third double roller (10) having a second temperature for cooling, and; - a removal of the sheet (1). 14- Method according to claim 13, wherein the application temperature of the component is equal to the first temperature. 15- Method according to any of claims 13 or 14, wherein the application of the component is carried out in a band (2) on the sheet (1) of paper and the band (2) has a width equal to the width of a reducing element of the application nozzle of the gun (6). 16- Method according to any of claims 13 or 14, wherein the component is applied discontinuously to the sheet of paper according to the pulses generated by an encoder of the gun (6). 17- Method according to any of claims 13 or 14, wherein the sheet (1) of paper comprises at least one print on its surface and the injection of component onto the knurled cylinder (8) comprises an initial reading step by means of a photocell of the gun (6) connected to the pump to determine the existence or absence of printing on the sheet (1) such that the pump is capable of stopping the injection of the gun (6) when it detects a print and activating the same when it detects the absence of printing. 18- Method according to any of claims 13 to 17, wherein the first application temperature of the component is between 100 and 110°

Citation Information

Patent Citations

  • Biodegradable article

    GB2612641A

  • Roduction of transparent paper

    JP1986132698A

  • Design paper

    JP1992136299A

  • Modified fibrous product and method of producing the same

    US20110256362A1

  • Machine for waxing paper

    US2081324A