Electrocatalytic mixed iron-vanadium oxide electrode, production method for same and its uses in hydrogen production
The mixed iron-vanadium oxide electrocatalytic electrode with a metal-organic matrix addresses the limitations of existing hydrogen production methods by reducing overpotential and enhancing current densities, offering a cost-effective and scalable solution for hydrogen production in various electrolysis processes.
Patent Information
- Application Number
- PCT/ES2024/070198
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Current electrocatalysts for hydrogen production in water electrolysis face challenges such as high energy consumption, costly materials like iridium and ruthenium, and scalability issues, particularly in alkaline and anion exchange membrane electrolysis, where the anode limits performance and requires corrosive conditions.
A mixed oxide electrocatalytic electrode comprising iron and vanadium in a non-stoichiometric form with a metal-organic matrix, which is only active under applied voltage, featuring a thin coating with a high organic content that forms porosity and enhances catalytic activity, reducing overpotential and improving current densities.
The electrocatalytic electrode achieves lower overpotential and higher current densities for hydrogen production, making it a viable alternative to expensive iridium and ruthenium oxides, suitable for alkaline and anion exchange membrane electrolysis, and capable of oxidizing alcohols with reduced energy consumption.
Smart Images

Figure ES2024070198_03102024_PF_FP_ABST
Abstract
Description
[0001] MIXED IRON-VANADIUM OXIDE ELECTROCATALYTIC ELECTRODE, PROCEDURE FOR ITS OBTAINING AND ITS USES IN HYDROGEN PRODUCTION
[0002] Field of the invention
[0003] The present invention falls within the field of electrocatalytic electrodes or electrocatalysts and their electrocatalytic coatings. In particular, the invention provides an electrocatalytic electrode of a mixed oxide comprising iron and vanadium for the production of molecular hydrogen.
[0004] Background of the invention
[0005] Today, there is a growing need to generate clean energy from renewable sources.
[0006] One source is the generation of hydrogen from water hydrolysis. Water hydrolysis occurs at room temperature using electrochemical methods with the following reactions:
[0007] 2H2O (I) 2H2(g) + O2(g) £°redox —-1,23V Hydrolysis
[0008] 2H + (aq) + 2e~ -> H2(g) £ o re d = 0 V Cathode (Water Reduction)
[0009] 2H2O (I) — *O2(g) + 4H + (aq) + 4e- £° ox = -1 .23 V Anode (Water Oxidation)
[0010] Electrochemical hydrolysis of water, known as electrolysis, occurs by applying a potential difference between two electrodes, the anode and the cathode. The reduction of water occurs at the cathode to produce H2 (Hydrogen Evolution Reaction, HER), and the oxidation of water occurs at the anode to produce O2 (Oxygen Evolution Reaction, OER). However, the electrolysis of water requires a large amount of extra energy in the form of overpotential, compared to the thermodynamically required 1.23 V, because the activation energy for the reaction must be exceeded. To reduce the overpotential, electrocatalysts are commonly used. These reduce the activation energy, thereby reducing the energy required to produce H2 and thus improving the reaction yield.
[0011] Alkaline electrolysis (AE) is suitable for both oxygen and hydrogen production. However, alkaline electrolysis uses highly basic pH compounds such as KOH. These basic compounds are highly corrosive and pose system maintenance problems because KOH is very sensitive to CO2 in ambient air and forms K2CO3, which lowers pH, blocks ion transfer channels, and limits current densities.
[0012] Polymer electrolyte membrane (PEM) electrolysis requires acidic conditions imposed by the proton exchange membrane (H + ), limiting the type of catalysts to noble metal materials and components such as Pt-coated Ti current collectors which are expensive.
[0013] An alternative, still in the pre-industrial stage, is electrolysis with anion exchange membranes (AEM). [I. Vincent, D. Bessarabov, Low cost hydrogen production by anion exchange membrane electrolysis: A review. Renew. Sust. Energy Rev. 2018, 81 , 1690-1704], These membranes can transport OH- instead of H + However, anion exchange membrane (AEM) electrocatalysts are still under development and require significant improvements in several aspects, such as energy efficiency, membrane and catalyst stability, ease of handling, and cost reduction in the manufacture of cells with anion exchange membrane catalysts that are scalable to industrial scale. It is also desirable for anion exchange membrane electrocatalysts to be capable of operating at significantly improved current densities to be a viable alternative for hydrogen production.
[0014] Recently, research has been conducted into the production of anodic electrodes for the oxidation of H2O because the anode limits the efficiency of water electrolysis. The oxidation reaction of water (anode) involves a greater number of species (4 electrons and 4 hydrogen atoms). + ) compared to the water reduction reaction (cathode) (2 electrons and 2 H + ). At the cathode, there are very low overpotentials compared to those at the anode. It is the anode that kinetically limits the electrochemical reaction to obtain oxygen and, therefore, also limits the efficiency of water electrolysis by electrocatalysis.
[0015] The selective electrocatalysts for water oxidation with the best performance to date include iridium oxides (I rO2) and ruthenium oxides (RUO2). Although these oxides are also useful for water reduction, the high cost of ruthenium and iridium is one of the main limitations for their implementation on an industrial scale. On the other hand, there are catalysts based on solid-state metal oxides that are cheaper than iridium and ruthenium, such as CoPi, Co-Bi, CoOx, MnOx, and NiOx. However, most of these alternative oxides to iridium and ruthenium are deposited on the substrate to obtain the electrocatalyst using chemical, electrochemical, physical methods such as sputtering, and photochemical deposition methods that are difficult to scale up to an industrial level and, therefore, not viable for obtaining molecular hydrogen on an industrial scale using these chemical techniques.
[0016] Patent CN 103974769 discloses a technique for obtaining metal oxides for catalytic purposes. However, the photochemical metal-organic deposition (PMOD) technique used uses ultraviolet (UV) radiation and is therefore not viable for industrial scale. The technique involves depositing a precursor and then irradiating it with UV light until all the organic material decomposes and forms metals in a metallic state, which are then oxidized at high temperatures. The production process eliminates any organic residue from the oxides formed, requires several stages, the use of UV light, and high temperatures, and is not suitable for industrial scale.
[0017] Patent EP0014596 discloses a method for producing electrodes with catalytic coatings of mixed metal oxides. Specifically, it discloses oxides of at least two metals obtained by thermal decomposition of organometallic compounds and a method for producing electrodes for electrolytic purposes with a coating that includes said oxides. The method has limitations in terms of scalability on an industrial scale. Furthermore, the purpose of thermal decomposition is to oxidize the metallic components to their oxide form. Therefore, it also does not disclose a metal-organic matrix with the presence of an organic component.
[0018] Patent EP2220000 relates to iron-doped vanadium (V) oxides of formula FeyV2O5, a production process and their uses, particularly in microbatteries. The process requires a spray chamber in which the starting components are sprayed together with a gas mixture at a certain pressure. It also requires the application of an electrical potential between the "V" target and the substrate, and a potential between the "Fe" target and the substrate for deposition. When using oxides, the V2O5 and Fe2O3 targets are pressurized and synthesized at a temperature of 400°C for 12 hours, and then at 600°C for 10 hours until a dense target with mechanical resistance is obtained. Thus, the heat treatment also eliminates any presence of organic material in the oxide obtained.Therefore, to date, the production of new metal oxides in a metal-organic matrix capable of producing hydrogen has not been described or suggested, nor has improved hydrogen production been described or suggested compared to methane reforming, which also has the disadvantage of leaving a significant carbon footprint.
[0019] It is desirable to provide clean energy to combat climate change by generating H2 capable of producing hydrogen with a lower reaction activation energy while leaving a zero-carbon footprint. H2 has applications, for example, as a fuel for generating electricity in a fuel cell, a very promising solution because it is a completely clean and recyclable energy source, as its combustion generates H2O as a product of the reaction, thus reducing the carbon footprint.
[0020] Therefore, there is a need to provide an improved electrocatalytic electrode or electrocatalyst for hydrogen production that overcomes at least one of the drawbacks of the prior art.
[0021] Description of the invention
[0022] In view of the state of the art, an objective of the present invention is to provide improved electrocatalysts based on metal oxides that are low cost, that can be manufactured by industrially scalable techniques and which techniques are also low cost.
[0023] Likewise, it is also the objective of the present invention to provide new electrocatalysts that have improved catalytic activity, adequate reaction yields and low energy consumption to produce molecular hydrogen.
[0024] Another objective of the present invention is to provide an electrocatalyst suitable for water electrolysis and alkaline water electrolysis (AE).
[0025] The present invention also aims to provide an electrocatalyst suitable for anion exchange membrane (AEM) electrolysis that is low-cost and provides good yields in obtaining molecular hydrogen. Another objective of the invention is to provide at least one process for obtaining the electrocatalytic electrode capable of being scalable at an industrial level, whose electrocatalytic electrode or electrocatalyst has application in at least water electrolysis, alkaline electrolysis (AE), anion exchange membrane (AEM) electrolysis, or photocatalysis.
[0026] With the electrocatalytic electrode or electrocatalyst of the invention, at least one of the aforementioned drawbacks is resolved, presenting other advantages that will be described below.
[0027] In a first aspect, the present invention provides a mixed oxide electrocatalytic electrode including iron and vanadium for hydrogen production.
[0028] The iron-vanadium mixed oxide electrocatalytic electrode comprises:
[0029] -an electrically conductive base substrate; and
[0030] -a coating film on the base substrate, comprising a coating, and characterized in that the mixed oxide is non-stoichiometric and includes a mixture of iron in oxidation state (II) and / or (III) and vanadium in oxidation state (IV) and / or (V), and in that the coating comprises a metal-organic matrix whose organic part includes the mixed oxide dispersed therein.
[0031] Advantageously, the presence of V(IV) and / or V(V) with Fe(ll) and / or Fe(lll) surprisingly improves the electrocatalytic properties of the electrode.
[0032] The structure of the mixed oxide described here includes a mixture of iron and vanadium. The iron and vanadium can be present in different percentages, expressed as a percentage of one. The mixed oxide can be represented by the general formula Fe a VbO x , where x denotes the oxygen atoms and has values between 1 and 2.5. The superscripts a and b indicate the atomic percentage expressed as percentages of iron and vanadium, respectively, and therefore the sum of a + b is equal to 1 .
[0033] Surprisingly, the electrocatalytic electrode of the first aspect of the invention is capable of generating vanadium oxide in the (V) oxidation state in combination with iron oxide in the (III) oxidation state in use, i.e., under an applied voltage or potential. Unexpectedly, the surface of the electrocatalytic electrode, i.e., the coating film or catalytic film, changes when a voltage or potential difference is applied: the Fe and V metals are completely oxidized and the coating film becomes active, acting as a catalyst.
[0034] Advantageously, the electrocatalytic electrode of the first aspect of the invention is not active without the passage of current (e ), application of voltage or potential difference.
[0035] The electrocatalytic electrode exhibits adequate chemical stability. This is believed to be due to the fact that the electrocatalytic electrode is only electrocatalytically active in use, under applied voltage or potential difference.
[0036] Advantageously, the coating film has improved catalytic properties.
[0037] The coating film may include one or several layers.
[0038] These layers may be identical or different. In the present invention, identical or different layers are understood as having the same or different composition, with composition being understood as the variation in the concentration of vanadium oxide (IV and V) and / or the variation in the concentration of iron oxide (II and III) and / or the organic material forming the organic part, and even the variation in the percentage of organic material present in the organic part of the coating film.
[0039] The first aspect of the invention provides an electrocatalytic electrode whose coating film or catalytic film is of reduced thickness, even with the presence of organic part in the film.
[0040] The coating film has a thickness of less than 1 nm. In particular, the coating film has a nanometer thickness. The thickness can range from 20 nm to 600 nm, preferably from 50 nm to 200 nm.
[0041] The coating film includes at least 10% by weight of organic matter relative to the total weight of the coating film. Between 15% and 30% by weight of organic matter relative to the total weight of the coating film is preferred. The remainder up to 100% is inorganic matter, which typically includes O' 2 and OH' among the most common.
[0042] The organic component acts as a support for the mixed oxide dispersed within it. The organic component comes from the anions of the iron or vanadium salts used to form the iron-vanadium mixed oxide.
[0043] The composition of the organic part in the metal-organic matrix comprises at least one organic compound selected from the group including an alkoxide, a carboxylate such as acetate, formate, oxalate, citrate, acetylacetonate, tartrate, an amine, a phosphonate, a sulfonate such as triflate or tosylate, or it may be a mixture of one or more thereof.
[0044] The inventors have found that the presence of the organic part in the coating film unexpectedly improves the catalytic properties of the electrocatalytic electrode in use, i.e., under applied voltage or potential difference.
[0045] Unexpectedly, the existence of this organic part in the coating film comprising the coating results in a decrease in the overpotential (mV) necessary for the oxidation reaction for the same current density (mA cm -2 ) applied.
[0046] Furthermore, surprisingly, when a voltage or potential difference is applied, pores are formed in said organic part, generating porosity in the coating film. Said porosity increases the catalytically active surface of the coating film and, in turn, that of the electrocatalytic electrode, according to the first aspect. The pores are a route for the entry and circulation of fluid (aqueous medium) through them, which increases the contact of the fluid with the catalyst, that is, with the mixed oxide dispersed in said organic part.
[0047] The mixed oxide has an amorphous structure.
[0048] In an X-ray diffraction test it was observed that the mixed oxide (Fea VbO x ) did not show any diffraction peaks, neither of FeO, Fe2Ü3 or FesCU, nor of V2O3 or V2O5. The absence of characteristic peaks of iron oxides (FeOx) nor of vanadium oxides (VOx) confirmed that the coating films or catalytic films include mixed oxide that includes a mixture of iron and vanadium oxides of amorphous structure (FIG 3).
[0049] In one embodiment, the mixed oxide consists of a mixture of iron in the (II) and / or (III) oxidation state and vanadium in the (IV) and / or (V) oxidation state. In the mixed oxide, the mixture of iron and vanadium is in a Fe:V molar ratio of between 9:1 and 1:9, preferably between 5:1 and 1:2.
[0050] In an optional embodiment, the mixed oxide including a mixture of iron and vanadium further includes in the mixture, forming part of the structure of the mixed oxide, at least one metal M selected from the group consisting of Ti, Cr, Mn, Co, Ni, Cu, Zn, Ga, Ge, Zr, Mo, Ru, Rh, Pd, Ag, In, Sn, W, Re, Os, Ir, Pt, Au and Ce.
[0051] In this optional embodiment, the mixed, non-stoichiometric oxide, which includes iron, vanadium and also at least one metal M can be represented by the general formula: Fe a VbM c Ox, where x indicates the oxygen atoms and has values between 1 and 3. The superscripts a, b and c indicate the atomic percentage expressed as a percentage of each metal in the mixed oxide structure and, therefore, the sum of a+b+c is equal to 1.
[0052] In a ternary mixture, iron, vanadium and metal M are in a molar ratio Fe:V:M between 9:0.5:0.5 and 2:5:3, preferably between 4:3:0.5 and 6:5:1.5, more preferably around 5:4:1.
[0053] In another different and also optional embodiment, combinable with or independent of the previous optional embodiment, the coating film may also include metal nanoparticles and / or nanoparticles of metal oxides other than iron and vanadium, optionally also other than the metal M which may include the mixed oxide structure according to the previous embodiment.
[0054] It is desirable that the nanoparticles do not include the metals that are part of the mixed oxide structure. The nanoparticles are dispersed in the organic part of the metal-organic matrix. The nanoparticles are dispersed independently of the mixed oxide, also dispersed in the organic part.
[0055] The nanoparticles are formed from salts and / or oxides of a metal selected from the group consisting of: Ti, Cr, Mn, Co, Ni, Cu, Zn, Ga, Ge, Zr, Mo, Ru, Rh, Pd, Ag, In, Sn, W, Re, Os, Ir, Pt, Au, and Ce, provided that the selected metal does not include any of the metals that form part of the mixed oxide structure: Fe, V, and optionally at least one additional metal M as defined above. Nanoparticles formed from salts and / or oxides of a metal selected from Ni, Au, Ag, Pd, Ru, and Ir, preferably Ni, Ru, Pd, and Ir, are preferred.
[0056] Advantageously, the presence of said metallic nanoparticles and / or metal oxides provides an electrocatalytic electrode with greater application versatility. Thus, according to the first aspect of the invention, an electrocatalytic electrode comprising a multifunctional coating film is also provided. The catalytic properties can be optimized by incorporating, for example, cocatalysts.
[0057] The electrically conductive base substrate may be made of a material that meets at least one of the following requirements: inorganic, organic, flexible, rigid, semi-rigid, transparent, opaque, solid or porous.
[0058] Advantageously, the structure and morphology of the coating film comprising a coating can employ a variability of electrically conductive base substrates.
[0059] Suitable base substrate materials include, as a non-limiting example of the invention, rigid or semi-rigid materials such as thin sheets of nickel, aluminum, steel or other porous metal supports such as metal foam such as nickel, steel or copper, nickel, steel or copper fiber paper and other types of rigid substrates such as glassy carbon, transparent substrates such as ITO and FTO on glass; flexible substrates such as ITO, FTO, and metals such as Au, Pt deposited on polymeric materials such as polyethylene terephthalate (PET), polyethylene phthalene (PEN), polypropylene (PP), polyethylene (PE), polyimide (Kapton Tape); or organic substrates such as cellulose.
[0060] The invention also relates to an electrocatalytic electrode obtainable by a wet deposition method. In particular, the coating film is obtained on the electrically conductive base substrate by a wet deposition method.
[0061] The various methods of wet coating on base substrates are generally known to those skilled in the art. Conventional techniques include spin coating, spray coating, dip coating, and Dr. Blade. Alternatively, the coating film can be obtained on the base substrate using roll-to-roll printing techniques such as slot-die coating, screen printing, and flexography.
[0062] In another alternative, the coating film can be obtained on the base substrate using digital printing techniques such as ink-jet printing.
[0063] As described above, the electrocatalytic electrode obtainable by a wet deposition method is preferable.
[0064] In a second aspect, the invention provides a process for obtaining an electrocatalytic electrode as defined in the first aspect of the invention which is carried out by wet method on an electrically conductive base substrate.
[0065] The process comprises the steps of: i-1) preparing a vanadium oxide precursor solution which includes selecting an organic or organic counter ion vanadium (II), (III), (IV), and / or (V) salt and dissolving the vanadium salt in a non-aqueous solvent; i-2) preparing an iron oxide precursor solution which includes selecting an iron (II) and / or (III) salt and dissolving the iron salt in a non-aqueous solvent;
[0066] (i) mixing the solutions prepared in steps i-1) - i-2) and depositing the mixture of solutions on the base substrate by a wet deposition method to obtain the coating film; and (iii) carrying out a thermal curing or first curing at a temperature between 20°C and 250°C to dry the coating film, which comprises the mixed oxide dispersed in the organic part of the metal-organic matrix.
[0067] The second aspect of the invention also relates to the preparation of the mixed oxide including a mixture of iron, vanadium and also at least one metal M selected from the group consisting of Ti, Cr, Mn, Co, Ni, Cu, Zn, Ga, Ge, Zr, Mo, Ru, Rh, Pd, Ag, In, Sn, W, Re Os, Ir, Pt, Au and Ce.
[0068] For each additional metal M added to the iron and vanadium mixture, the process further comprises repeating step i-3) [i-3n)] below:
[0069] - i-3), preparing a precursor solution of a metal oxide from one or more salts and / or one or more oxides of the metal M in a non-aqueous solvent to obtain the solution of one or more salts and / or one or more oxides of the metal M and then, in step ¡i), the solution prepared in step i-3) is mixed with the prepared solutions of vanadium i-1) and iron i-2), and proceeding to step iii), i.e. with a first thermal curing.
[0070] The second aspect of the invention also relates to the preparation of nanoparticles of metals and / or metal oxides, other than iron and vanadium, from a metal selected from the group consisting of: Ti, Cr, Mn, Co, Ni, Cu, Zn, Ga, Ge, Zr, Mo, Ru, Rh, Pd, Ag, In, Sn, W, Re, Os, Ir, Pt, Au, and Ce.
[0071] To form the nanoparticles, the process also includes the following step i-4):
[0072] - i-4) preparing a solution of one or more metal salts and / or one or more metal oxides from one or more salts and / or one or more oxides of at least one metal selected from the group consisting of Ti, Cr, Mn, Co, Ni, Cu, Zn, Ga, Ge, Zr, Mo, Ru, Rh, Pd, Ag, In, Sn, W, Re, Os, Ir, Pt, Au and Ce in a non-aqueous solvent; in step ¡i), the solution or solutions prepared in step i-4) are mixed with the solutions prepared in steps i-1) and i-2), and optionally with the solution or solutions prepared in step i-3) [i-3n)].
[0073] For the formation of nanoparticles, in stage iii), a second thermal curing is required after performing the first thermal curing.
[0074] The second curing is carried out at a temperature higher than that of the first curing and lower than 350°C.
[0075] It is preferred that the first curing be carried out at a temperature below 100°C and the second curing at a temperature above 100°C and below 350°C, preferably above 200°C and below 350°C.
[0076] The coating film may include metal nanoparticles and / or nanoparticles of metal oxides other than iron and vanadium dispersed, independently of the mixed oxide, in the organic part of the metal-organic matrix.
[0077] In step i), precursor solutions of the oxides of the metals that form part of the structure of the mixed oxide are prepared from a salt of the metal. Thus, in step i), precursor solutions of vanadium oxides i-1) and iron i-2) and, optionally, of other oxides i-3), i-31), i-32), i-3n) other than iron and vanadium defined above in the first aspect are prepared from a salt of the oxide.
[0078] The solutions are prepared in a non-aqueous solvent independently selected from glycol ethers, glycol ether acetates, and derivatives or mixtures thereof. "Independently" indicates that each solution can be prepared, if desired, with a different non-aqueous solvent.
[0079] The preferred non-aqueous solvent is selected from one of the following: 2-Methoxyethanol, 2-Ethoxyethanol, 2-Butoxyethanol, 2-(2-Ethoxy-ethoxy)ethanol, 2-Propoxyethanol, 2-Isopropoxyethanol, 2-Benzyloxyethanol, 2-(2-Methoxyethoxy)ethanol and 2-(2-Butoxyethoxy)ethanol.
[0080] The solution of the vanadium (II) (III) (IV) and / or (V) salt can be prepared at a concentration equal to or greater than 0.05M, preferably at a concentration between 0.1M and 3M.
[0081] Preferably, the vanadium salt is a vanadium(V) salt.
[0082] The organic counterion vanadium(V) salt may be selected from vanadium tripropoxide, vanadium triisopropoxide, and vanadium triethoxide. Preferably, the organic counterion vanadium(V) salt is at a concentration of between 0.1 M and 3 M.
[0083] The inorganic counterion vanadium(V) salt may be selected from vanadium trichloride oxide, sodium orthovanadate, sodium metavanadate, potassium metavanadate, cesium metavanadate.
[0084] The inorganic counterion vanadium(IV) salt as vanadium sulfate oxide
[0085] The organic counterion vanadium(III) salt as vanadium acetylacetonate.
[0086] The inorganic counterion vanadium(III) salt as vanadium trichloride.
[0087] The inorganic counterion vanadium(II) salt as vanadium chloride.
[0088] The iron (II) and / or (III) salt may be selected from chloride, perchlorate, p-toluenesulfonate, acetate, formate, oxalate, acetylacetonate, tartrate, or citrate. The solution of the iron (II) and / or (III) salt may be prepared at a concentration equal to or greater than 0.05M, preferably at a concentration between 0.1M and 3M.
[0089] The solution of the salt of another metal M other than iron and vanadium can be prepared following the same methodology and range of concentrations defined for vanadium and iron.
[0090] The concentration of each metal in solution determines the percentage in percent of the general formula of the mixed oxide: Fe a VbOx or Fe a VbM c Ox.
[0091] As described above, iron and vanadium can be present in different percentages or molar ratios.
[0092] In one embodiment, the mixed oxide consists of a mixture of iron and vanadium (Fe a VbOx). The percentage of vanadium may be between 5% and 95%, preferably between 30% and 40%, with the remainder up to 100% being iron. In this embodiment, the iron and vanadium may be in a Fe:V molar ratio of between 9:1 and 1:9, preferably between 5:1 and 1:2.
[0093] For water electrolysis, it is preferred that iron be in excess of vanadium. Vanadium is preferably present at a concentration between 30% and 40%, with the remainder being up to 100% iron. This percentage range in the general formula is represented as follows: FeOjVo.sOx to FeO,6Vo,40x.
[0094] In another embodiment, the mixed oxide includes a mixture of iron, vanadium and another metal M in the structure with general formula: Fe a VbM cOx. FIG. 14 shows an embodiment where the other metal M is Zn, obtained according to Example 4. The mixed oxides: FeO,5Vo,4ZnO,iOx, FeO,sVo,sZnO^Ox and FeO,4Vo,4ZnO,20x, shown in FIG. 14, were obtained by varying the concentration of each metal in the precursor solution of the oxide of the corresponding metal.
[0095] In another embodiment, the coating film may include nanoparticles.
[0096] For the preparation of the nanoparticles, in this step (i), a solution of one or more metal salts and / or one or more metal oxides is prepared from one or more salts and / or one or more oxides of at least one metal selected from the group of metals for nanoparticles described above in the first aspect. The solution is prepared in a non-aqueous solvent selected from those described herein.
[0097] Stage ¡i)
[0098] In step i) the solutions prepared in step i) are mixed.
[0099] The mixture of solutions is poured or deposited onto the electrically conductive base substrate to obtain the coating film.
[0100] A wet deposition method is preferred for depositing the solution mixture onto the base substrate.
[0101] Advantageously, the wet deposition method is scalable at an industrial level and low-cost to manufacture, and allows for the easy depositing of one or more layers.
[0102] In an optional embodiment, the solution mixture is heated to form an aged solution mixture. Heating temperatures between 30 and 80°C are preferred.
[0103] Stage iii)
[0104] In stage iii) at least one thermal curing of the coating film from stage ¡i) is carried out.
[0105] Curing or first thermal curing is carried out at a temperature between 20°C and 250°C.
[0106] Thermal curing or initial curing at a temperature between 20°C and 200°C is preferred. The upper temperature range is limited by the calcination temperature of the organic material so that the coating film contains an organic component. The curing time depends on the thermal curing temperature and can range from a few minutes to a few hours.
[0107] The organic part comes from the anions of the iron and / or vanadium salts selected in the stages of preparation of the solutions [i-1 ) and / or i-2)]. Thus, the nature of the organic part determines the calcination temperature, although a temperature below 250°C, preferably below 200°C ensures the presence of an organic part in the metal-organic matrix. Advantageously, the curing or first curing temperatures ensure the existence of an organic part in the coating film and, therefore, ensure the formation of pores in the coating film.
[0108] Contrary to what might be expected, relatively low curing temperatures, compared to the prior art temperatures, provide an electrocatalytic electrode comprising the coating film with improved catalytic properties and adequate stability of the coating film.
[0109] In the prior art, it is preferred to remove any remaining organic material using elevated temperatures during electrode fabrication. Although catalysts that include pores have been described, the films must be micron-thick because at thinner films, there is insufficient space for the pore voids, and compaction occurs very quickly. This is preferable in the prior art because compaction is believed to improve catalytic properties and increase catalyst stability.
[0110] Advantageously, with the method defined in the second aspect of the invention, the electrocatalytic electrode is provided comprising the coating film, which comprises the coating, with a metal-organic matrix whose organic part represents at least 10% by weight with respect to the total weight of the coating film and with the mixed oxide that includes a mixture of iron and vanadium dispersed in said organic part.
[0111] In a third aspect, the invention relates to the use of the electrocatalytic electrode or electrocatalyst defined in the first aspect as an electrocatalytic electrode for the production of molecular hydrogen.
[0112] Thus, the electrocatalytic electrode comprises the coating film with the mixed oxide that includes a mixture of iron and vanadium, and optionally at least one additional metal M, as an electrocatalytic electrode for the electrolysis of water by water oxidation.
[0113] In one embodiment, the electrocatalytic electrode comprises the coating film with the mixed oxide consisting of a mixture of iron and vanadium. Advantageously, the electrode has an overpotential of approximately [0.47 V (overpotential 0.24 V)] at 10 mA / cm 2 by the oxidation of water.
[0114] In another embodiment, the electrocatalytic electrode comprises the coating film with the mixed oxide that includes a mixture of iron and vanadium, and optionally at least one additional metal M, as described herein. This embodiment is especially suitable for application of the electrocatalytic electrode in alkaline water electrolysis (AE).
[0115] Advantageously, the electrocatalytic electrode or electrocatalyst is capable of catalyzing the alkaline electrolysis of water in a 3-electrode cell at a potential of approximately 1.47 V at 10 mA cm -2 (overpotential 0.24V) and a current density of 1 A / cm 2 at 2 V.
[0116] In another embodiment, the electrocatalytic electrode comprising the coating film with the mixed oxide that includes a mixture of iron and vanadium, and optionally at least one additional metal M, has application as an electrocatalytic electrode in alkaline anion exchange electrolysis (AEM). Advantageously, significantly improved current densities are obtained with the electrocatalytic electrode of the first aspect for hydrogen production.
[0117] Advantageously, the electrocatalytic electrode or electrocatalyst is capable of catalyzing the alkaline electrolysis of water in AEM cell at a potential of approximately 1.4 V at 10 mA cm -2 (overpotential 0.11 V) and a current of 4 A at 2 V.
[0118] In yet another embodiment, the electrocatalytic electrode comprising the coating film with the mixed oxide including a mixture of iron and vanadium, and optionally at least one additional metal M, is applicable as a selective electrocatalytic electrode. Therefore, the electrocatalytic electrode of the first aspect can replace the electrocatalysts known to date based on iridium oxides (IrO2) and ruthenium oxides (RUO2). An electrocatalytic electrode capable of selectively oxidizing water with improved hydrogen production yields compared to those obtained with the selective electrodes of iridium oxides (IrC>2) or ruthenium oxides (RUO2) known to date has not been described in the prior art.
[0119] In another embodiment, the electrocatalytic electrode comprising the coating film with the mixed oxide that includes a mixture of iron and vanadium, and optionally at least one additional metal M, is used as an electrocatalytic electrode in the electrolytic oxidation of organic compounds. An electrocatalytic electrode capable of selectively oxidizing alcohols in an aqueous medium with higher hydrogen production yields than those obtained in the selective oxidation of water for the production of molecular hydrogen has not been described in the prior art.
[0120] The electrocatalytic electrode defined in the first aspect of the invention also has application as an anode to carry out oxidation reactions other than the oxidation of water at said anode.
[0121] The electrocatalytic electrode is used for the oxidation of alcohols, for example, glycerol. At the anode, the alcohol oxidation reaction is energetically more favorable than the oxidation of water. This is due to the fact that alcohols are oxidized at a lower potential than water and, therefore, requires less electrical energy. Therefore, glycerol-assisted H2 generation can be achieved at a low energy cost and can also convert low-value-added waste such as glycerol into high-value-added products at the anode, with H2 production at the cathode. Glycerol is a byproduct in biodiesel production, where 1 ton of biodiesel production produces approximately 100 kg of glycerol. The rapid development of the biodiesel industry in recent decades has led to a significant oversupply of glycerol on the global market.Fortunately, glycerol is a highly functionalized molecule with three hydroxyl groups, which facilitates its valorization into more cost-effective chemical products. Most of the compounds obtained from glycerol oxidation are commercially relevant, especially those containing three carbon atoms, such as dihydroxyacetone, hydroxypyruvic acid, glyceraldehyde, glyceric acid, and low-cost tartronic acid.
[0122] Advantageously, the electrocatalytic electrode has a potential of approximately 1.33 V at 10 mA / cm 2 by electrolysis of water by oxidation of glycerol.
[0123] Therefore, the electrocatalytic electrode defined here also solves the additional problem of converting low-value-added alcoholic byproducts from biodiesel production, such as glycerol, into high-value-added products. Thus, the electrocatalytic electrode according to the first aspect of the invention is a good substitute for platinum, currently one of the most efficient catalysts for the oxidation of alcohols, which is also a transition metal from the group of noble metals that is very rare in the Earth's crust and extremely expensive.
[0124] The electrocatalytic electrode according to the first aspect of the invention has application as an electrocatalytic electrode for the oxidation of organic compounds that include derivatives of glycerol and / or lignocellulose.
[0125] In another embodiment, the electrocatalytic electrode has application in photocatalysis.
[0126] Thus, the electrocatalytic electrode according to the first aspect is a viable alternative for the oxidation of water to O2 with low overpotentials for alkaline water electrolysis, achieving good reaction yields, low material cost for obtaining the electrocatalyst, and ease of manufacture using low-cost techniques. Furthermore, the electrocatalytic electrode is also suitable as an anode for both conventional alkaline electrolysis and alkaline anion exchange electrolysis.
[0127] Anion exchange membrane electrolysis has clear advantages over other electrolytic processes such as conventional alkaline electrolysis (AE) or the more recent proton exchange membrane (PEM) electrolysis method, which relies heavily on raw materials such as precious metals.
[0128] As described above, the electrocatalytic electrode of the first aspect is also suitable for the oxidation of alcohols such as glycerol in aqueous solution at lower potentials than for the oxidation of H2O to O2.
[0129] Definitions
[0130] In the present invention, the terms “electrocatalyst” and “electrocatalytic electrode” have been used interchangeably and with the same meaning.
[0131] In the present invention, the terms “coating film” and “catalytic film” have been used interchangeably and with the same meaning.
[0132] Brief description of the Figures For a better understanding of what has been explained, some drawings are attached which, schematically and only as a non-limiting example, represent a practical case of implementation.
[0133] Figure 1 shows a graph of the UV-Visible-IR absorption spectrum of the electrocatalytic electrode comprising the coating film obtained according to Example 1 versus different curing temperatures.
[0134] Figure 2 shows a graph with the electrical resistance of the electrocatalytic electrode comprising the coating film obtained according to Example 1 versus different curing temperatures.
[0135] Figure 3 shows a graph of the X-ray diffraction spectrum of the electrocatalytic electrode coating film obtained according to Example 1 versus different curing temperatures, from 150°C to 500°C. It is observed that the mixed, non-stoichiometric oxide has an amorphous structure.
[0136] Figure 4 shows a scanning electron microscope (SEM) image of the cross section of the electrocatalytic electrode comprising the coating film, showing a film thickness of 130 nm, obtained according to Example 1 and a curing temperature of 200°C.
[0137] Figure 5 shows two images (A, C) obtained with a scanning electron microscope of the surface of the coating film and two graphs (B, D), respective to the images, obtained by means of X-ray microanalysis coupled to the SEM. Image -A- shows the surface of the coating film comprising dispersed the mixed oxide consisting of a mixture of iron and vanadium, obtained according to Example 1 using first curing temperatures of 200°C and without applying voltammetric cycling (CV) versus image -C- which shows the surface of the coating film comprising dispersed the mixed oxide including a mixture of iron, vanadium and also Zn, obtained according to Example 4 using first curing temperatures of 200°C and after having applied CV (postmortem).Graphs -B- and -D- show respectively the X-ray spectra of the coating film -A- without applying voltammetric cycling (CV) versus that of the coating film -C- after having applied CV (post-mortem). Figure 6 shows two graphs (A, B): graph -A- shows the current densities in the alkaline electrolysis of water, in a three-electrode cell, using the electrocatalytic electrode that includes the coating film obtained according to Example 1, with variations in the weight percentage of vanadium in the iron and vanadium mixture in the mixed oxide structure, and with a curing temperature of 250°C, first cure; graph -B- shows the overpotentials of the electrocatalytic electrode of -A- for different current densities of 10, 100 and 500 mA cm. -2 and different weight percentages of vanadium (% V) with respect to the weight of the mixed oxide.
[0138] Figure 7 shows two graphs (A, B): graph -A- shows the current densities (mA cm -2 ) in the alkaline electrolysis of water, in a three-electrode cell, using the electrocatalytic electrode comprising the coating film obtained according to Example 1, for different curing temperatures, first curing, of 100°C, 150°C, 200°C and 250°C; graph -B- shows the overpotentials of the electrocatalytic electrode comprising the electrocatalytic coating film according to the different curing temperatures, first curing, for different current densities of 10, 100 and 500 mA cm -2 .
[0139] Figure 8 shows a chronopotentiometry, with a constant current intensity at 10 mA cm -2, from the alkaline electrolysis of water, in a three-electrode cell, using the electrocatalytic electrode comprising the electrocatalytic coating film obtained according to Example 1 of the invention, with 40% by weight of vanadium and with a curing temperature of 250°C.
[0140] Figure 9 shows images obtained with a scanning electron microscope, where image A corresponds to the surface of a nickel sponge substrate without depositing the electrocatalytic coating and without a curing stage; and image B corresponds to the surface of the electrocatalytic coating film obtained according to Example 2 with 40% by weight of vanadium and with a curing temperature of 200°C.
[0141] Figure 10 shows in A a graph of the alkaline electrolysis of water in a three-electrode cell using the electrocatalytic electrode comprising the coating film obtained according to Example 2 with 40% by weight of vanadium and with a curing temperature of 200°C versus an undeposited nickel sponge substrate without thermal curing; and in B a bar diagram showing the overpotentials for different current densities of 10, 600 and 1000 mA cm -2 on the electrocatalytic electrode comprising the coating film versus the untreated nickel sponge substrate.
[0142] Figure 11 shows a graph of the alkaline electrolysis of water in a two-electrode cell with a “sandwich” configuration with an anion exchange membrane between both electrodes, using the electrocatalytic electrode comprising the coating film, obtained according to Example 2 with 40% by weight of vanadium and with different curing temperatures of 200°C and 250°C, versus an undeposited nickel sponge substrate without thermal curing.
[0143] Figure 12 shows images obtained with a scanning electron microscope showing in A the surface of an undeposited and non-thermal cured nickel fiber paper substrate versus B showing the surface of the electrocatalytic coating film obtained according to Example 3 with 40% by weight of vanadium and with a curing temperature of 250°C.
[0144] Figure 13 shows in A a graph of the alkaline electrolysis of water in a three-electrode cell using the electrocatalytic electrode comprising the coating film, obtained according to Example 3 with 40% by weight of vanadium and with a curing temperature of 250°C, versus an undeposited nickel fiber paper substrate without thermal curing; and in B a bar diagram with the overpotentials for different currents of 10, 600 and 1000 mA cm -2 on the electrocatalytic electrode comprising the coating film versus the untreated nickel fiber paper substrate.
[0145] Figure 14 shows in A a graph of water hydrolysis using the electrocatalytic electrode comprising the coating film obtained according to Example 4, which includes different concentrations of Zn; and in B a graph with the overpotentials of the electrocatalytic electrode comprising the coating film for different currents of 10, 100 and 500 mA cm -2 in the different mixed oxides that include a mixture of iron and vanadium and also Zn in the mixed oxide structure.
[0146] Figure 15 shows in A a graph of the alkaline electrolysis of water in a three-electrode cell using the electrocatalytic electrode comprising the coating film obtained according to Example 5 with 40% by weight of vanadium and with a curing temperature of 250°C with a 1M KOH electrolyte in the presence of 0.1M glycerol versus using the same electrolyte and concentration but without glycerol; and in B shows a bar chart with the comparative overpotentials for different current densities of 10, 50, 100, 300 and 500 mA cm -2 with and without the presence of glycerol.
[0147] Figure 16 shows a bar diagram of the overpotential (V) of the state-of-the-art oxides in 1 M NaOH at 10 mA cm -2described by McCrory et al in “Benchmarking Heterogeneous Electrocatalysts for the Oxygen Evolution Reaction" in J. Am. Chem. Soc. 2013, 135, 16977-16987, also includes the overpotential of the mixed oxides within the scope of the attached claims (first two bars) for the purpose of comparison with the overpotentials of the oxides of the state of the art.
[0148] Preferred embodiments for carrying out the present invention are described below.
[0149] Examples
[0150] Example 1 - Electrocatalytic electrode with mixed oxide Fe-V on a non-porous substrate - Initially, the precursor solutions of iron and vanadium were prepared. On the one hand, a 1 M solution of vanadium(V) triisopropoxide (1.22 g) in methoxyethanol (V=5 mL) was prepared. On the other hand, a 1 M solution of iron(III) chloride (0.811 g) in methoxyethanol (V=5 mL) was prepared. The solutions were mixed.
[0151] A thin film of FeVOx was then deposited on a glass substrate by spin coating at a speed of 2,000 rpm for 30 s. FIG. 1 shows the absorption spectrum for different curing temperatures carried out over a period of 30 min at that temperature.
[0152] Figure 1 shows that the material exhibits two absorption ranges: one in the IR (900 to 1,800 nm) and another in the visible range of 400-500 nm (hence its yellowish color), which overlaps with the absorption of glass starting at 350 nm. Above 200°C, the material exhibits absorption throughout the visible range, turning grayish.
[0153] The electrical resistance of the catalytic film was measured at different curing temperatures (see FIG. 2). It was observed that there is an inflection point at 200°C, where the material begins to turn grayish, as previously mentioned, and the resistance decreases considerably, nearly three orders of magnitude, from 5 GQ to approximately 5 MQ for a curing temperature of 250°C. It was also observed that, as the temperature increased further, the material's resistance rose again to above 150 MQ.
[0154] In order to determine the crystallinity of the non-stoichiometric iron-vanadium mixed oxide formed in the catalytic film, an X-ray diffraction test was performed for different curing temperatures (see FIG 3).
[0155] It was observed that at different curing temperatures from 150°C to 500°C, FeVO xdid not show diffraction peaks, neither of FeO, Fe2O3, FesC, nor of V2O3, V2O5. The absence of characteristic peaks of FeO x or VO X confirmed that the FeVO films x They were formed by an amorphous structure comprising a mixture of iron and vanadium oxides.
[0156] Determination of coating film thickness
[0157] To determine the thickness of the spin-coating layers, images were taken with a scanning electron microscope (SEM) (see FIG. 4). FIG. 4 shows that the material is less than 150 nm thick at a curing temperature of 200°C, confirming the production of a very thin layer of material.
[0158] Porosity
[0159] On the other hand, photographs were taken of the surface of an unused coating film and of a coating film after alkaline water electrolysis, and their respective X-ray microanalysis coupled with SEM was performed (see FIG. 5). It was seen that after performing the electrolysis tests, voids were generated in the layer, creating porosity that increases the catalytically active surface area. Furthermore, microanalysis showed that some of the vanadium dissolved during alkaline water electrolysis (Table 1).
[0160] Table 1. Fe and V composition (in % of atoms) of the catalytic film before and after applying cyclic voltammetry for alkaline water electrolysis. The catalytic properties of the catalytic film obtained in a 3-electrode electrochemical cell with 1 M KOH electrolyte were continued with a test. The overpotential required to reach current densities of 10 mA / cm was taken as the most representative measure of the catalytic activity. 2 (although overpotentials at 100 and 500 mAcm are also shown) -2 to better understand the differences between materials). The overpotential is defined as the excess energy that must be applied for the reaction to occur, i.e., the activation energy. In general, all chemical reactions have an activation energy. Catalysts reduce this activation energy. In electrochemical terms, the activation energy can be somewhat equated with the overpotential.
[0161] Therefore, the overpotential required to perform water electrolysis was checked using an electrocatalytic electrode with a base substrate consisting of a nickel foil with the coating film or catalytic film. The overpotentials obtained were in the order of 0.24-0.25 V (240-250 mV) (see FIGS 6, 7, 8 and 9) which proved to improve the overpotentials measured with reference materials such as Ir and Ru oxides (see FIG 10), where specifically IrOx (non-stoichiometric iridium oxide) shows an overpotential of 0.33 V. Furthermore, it is also necessary to look at the current reached at higher overpotentials, since the higher the current reached, the greater the hydrolysis of water and, consequently, more oxygen and hydrogen will be produced.As can be seen in FIGS 6 and 7, the overpotential and maximum current presented by the catalytic film can vary depending on the weight percentage of the components and / or the curing temperature to which it has been subjected.
[0162] Stability of the coating film
[0163] Also, the stability of the catalytic film was studied over 48 hours of continuous work by means of chronopotentiometry, maintaining a current of 10 mAcm -2 . In FIG. 8, it can be seen that the measurement remains practically constant (there is barely a 1% increase in potential), so the catalytic film remains stable and is working without decreasing its catalytic activity over time.
[0164] Example 2 - Electrocatalytic electrode with Fe-V mixed oxide on porous substrate - Electrolysis of alkaline water - Catalytic properties test
[0165] Initially, the precursor solutions of iron and vanadium were prepared. First, a 1 M solution of vanadium(V) oxide thisopropoxide (1.22 g) in methoxyethanol (V=5 ml) was prepared. Secondly, a 1 M solution of iron(III) chloride (0.811 g) in methoxyethanol (V=5 mL) was prepared. The solutions were mixed.
[0166] FeVOx was further deposited on a porous nickel sponge substrate by dip coating, leaving it submerged for 1 minute, then drying by capillarity and, finally, by spin coating at 2,000 rpm for 30 seconds. Figure 9 shows two images obtained by scanning electron microscope: one of a nickel sponge substrate without deposited material (FIG 9A) and another of a nickel sponge substrate on which FeVOx has been deposited by dip coating, has been dried by capillarity and by spin coating and, finally, has been subjected to thermal curing at 200 degrees for 30 minutes (FIG 9B).
[0167] In Figure 9, the porous structure of the nickel sponge and, consequently, its larger catalytically active surface area are clearly visible. Furthermore, the material is seen depositing throughout the substrate, even blocking some of these pores. Therefore, the amount of material deposited on a nickel sponge of a given size will be greater than that deposited on a nickel foil of the same size, and therefore its catalytic activity for water electrolysis will be higher.
[0168] To verify this, a test of the catalytic properties of the catalytic film obtained in a 3-electrode electrochemical cell with 1 M KOH electrolyte was carried out. As in example 1, the overpotential necessary to reach current densities of 10 mA / cm was taken as the most representative measure of the catalytic activity. 2For this purpose, an electrode consisting of a nickel sponge with the catalytic film was used for the electrolysis of alkaline water in a three-electrode cell. The overpotentials obtained were of the order of 0.2 V (see FIG. 10), i.e., approximately 50 mV less than those obtained in Example 1 with the nickel foil electrode with the catalytic film. Furthermore, currents of 1.4 A cm were achieved. -2 at potentials of 2 V vs NHE (FIG. 10), much higher than with the nickel foil (FIGS. 6 and 7). Therefore, using the nickel sponge with the catalytic film results in lower overpotentials and better currents, i.e., a greater amount of hydrogen is produced.
[0169] Anion exchange cell electrolysis (AEM)
[0170] Alkaline water electrolysis was tested in a two-electrode anion exchange cell (AEM) with a sandwich configuration, in which an anion exchange membrane is sandwiched between the electrodes. This type of assembly is called an AEM cell. Figure 11 shows that the nickel sponge with the catalytic film, thermally cured at 200°C, reaches currents of 4.5 A / cm , more than four times higher than those achieved by the nickel sponge without the catalyst. In other words, reaching such high currents increases the generation of hydrogen by water electrolysis.
[0171] Example 3 - Electrocatalytic electrode with Fe-V mixed oxide on porous substrate - Electrolysis of alkaline water - Catalytic properties test
[0172] Initially, the precursor solutions of iron and vanadium were prepared. First, a 1 M solution of vanadium(V) triisopropoxide (1.22 g) in methoxyethanol (V=5 mL) was prepared. Secondly, a 1 M solution of iron(III) chloride (0.811 g) in methoxyethanol (V=5 mL) was prepared. The solutions were mixed.
[0173] FeVOx was further deposited on a porous nickel fiber paper substrate by dip coating, leaving it submerged for 1 minute, then drying by capillarity and, finally, by spin coating at 2,000 rpm for 30 seconds. FIG. 12 shows two images obtained by scanning electron microscope: one of a nickel fiber paper substrate without deposited material (FIG. 12A) and another of a nickel fiber paper substrate on which FeVOx has been deposited by dip coating, dried by capillarity and by spin coating and, finally, subjected to thermal curing at 250°C for 30 minutes (FIG. 12B).
[0174] In FIG. 12, the structure of the substrate is clearly visible, where the nickel fibers are intertwined with each other. This gives the nickel fiber paper a certain porosity and permeability, allowing the passage of electrolyte or gases. Furthermore, the material (FeVOx) is deposited as a layer covering the nickel strands, without blocking the gaps between the filaments and, therefore, does not affect the porosity and / or permeability of the substrate.
[0175] A test of the catalytic properties of the catalytic film obtained was carried out in a 3-electrode electrochemical cell with 1 M KOH electrolyte. As in examples 1 and 2, the overpotential necessary to reach current densities of 10 mA / cm was taken as the most representative measure of the catalytic activity. 2For this purpose, an electrode consisting of nickel fiber paper with the catalytic film was used for the electrolysis of alkaline water in a three-electrode cell. The overpotentials obtained were around 0.23 V for current densities of 10 mA / cm. 2 and the currents reached were 1.1 A cm -2 at 2V vs NHE (see FIG 13), these are data very similar to those obtained in example 1 using a nickel foil with the catalytic film as an electrode.
[0176] The advantages of this substrate over nickel foil are that it can be heated to higher temperatures without oxidizing the substrate in the process and that it can be used as a gas diffusion layer (GDL).
[0177] Compared to nickel sponge, it only has the first advantage, since nickel sponge can also be used as a GDL and also achieves better overpotentials and currents.
[0178] Example 4 - Electrocatalytic electrode with mixed oxide Fe-V-Zn on non-porous substrate - Electrolysis of alkaline water
[0179] Initially, the precursor solutions of iron, vanadium and zinc were prepared. First, a 1 M solution of vanadium(V) triisopropoxide (1.22 g) in methoxyethanol (V=5 mL) was prepared. Secondly, a 1 M solution of iron(III) chloride (0.811 g) in methoxyethanol (V=5 mL) was prepared. Finally, a 1 M solution of zinc(II) nitrate (0.947 g) in methoxyethanol (V=5 mL) was prepared. The solutions were mixed.
[0180] A thin film of ZnFeVOx was then deposited on a nickel foil substrate by spin coating at a speed of 2,000 rpm for 30 seconds.
[0181] The catalytic properties of the catalytic film obtained were checked in a 3-electrode electrochemical cell with 1 M KOH electrolyte. The overpotential required to reach current densities of 10 mA / cm was taken as the most representative measure of the catalytic activity. 2 . For this purpose, an electrode consisting of a nickel foil with the catalytic film (ZnFeVOx) was used for the electrolysis of alkaline water in a three-electrode cell. In FIG. 14, it can be seen that by adding Zn to the reaction mixture, very good catalytic properties can be obtained with overpotentials of up to 240 mV of the film, reaching currents of 1 Acm. -2 a 2V vs NHE.
[0182] Oxidation of alcohols Initially, the precursor solutions of iron and vanadium were prepared. First, a 1 M solution of vanadium(V) triisopropoxide (1.22 g) in methoxyethanol (V=5 mL) was prepared. Secondly, a 1 M solution of iron(III) chloride (0.811 g) in methoxyethanol (V=5 mL) was prepared. The solutions were mixed.
[0183] A thin film of FeVOx was then deposited on a nickel foil substrate by spin coating at a speed of 2,000 rpm for 30 seconds.
[0184] The presence of an alcohol, such as glycerol, in the electrolyte can make H2 production more energetically favorable. This is because the oxidation of alcohols occurs at lower potentials than the oxidation of water and, consequently, electrolysis requires less electrical energy. In addition, it converts low-value waste such as glycerol into high-value-added products at the anode, producing H2. To verify this, two catalytic property tests were carried out in a 3-electrode electrochemical cell using the same nickel foil electrode with the catalytic film (FeVOx). In one of the tests, alkaline water (1 M KOH) was used as the electrolyte, and in the other test, alkaline water (1 M KOH) was used with glycerol dissolved at a concentration of 0.1 M.
[0185] In FIG 15, it was found that the presence of glycerol significantly reduces the potential required to carry out the oxidation at the anode (1.35 V in the presence of glycerol, compared to 1.5 V without glycerol for a current of 10 mA / cm 2 ). Therefore, the use of alcohol significantly reduces the energy consumption required for H2 generation and also converts waste into products of industrial interest.
[0186] Although reference has been made to a specific embodiment of the invention, it is evident to a person skilled in the art that the optional features are susceptible to numerous variations and modifications, and that all the details mentioned may be replaced by other technically equivalent ones, without departing from the scope of protection defined by the appended claims.
Claims
CLAIMS 1. Mixed iron-vanadium oxide electrocatalytic electrode comprising: -an electrically conductive base substrate; and -a coating film on the base substrate, comprising a coating, characterized in that the mixed oxide is non-stoichiometric and includes a mixture of iron in oxidation state (II) and / or (III) and vanadium in oxidation state (IV) and / or (V), and in that the coating comprises a metal-organic matrix whose organic part includes the mixed oxide dispersed therein.
2. Electrocatalytic electrode according to claim 1, wherein the coating film includes one or more layers.
3. Electrocatalytic electrode according to any one of claims 1-2, wherein the coating film is of nanometric thickness.
4. Electrocatalytic electrode according to any one of claims 1-3, wherein the coating film has a thickness between 20 nm and 600 nm, preferably between 50 nm and 200 nm.
5. Electrocatalytic electrode according to claim 1, wherein the coating film includes at least 10% by weight of organic part with respect to the total weight of the coating film.
6. Electrocatalytic electrode according to claim 5, wherein the coating film includes between 15% and 30% by weight of organic part with respect to the total weight of the coating film.
7. Electrocatalytic electrode according to any one of claims 1, 5-6, wherein the organic part comprises at least one organic compound selected from the group that includes an alkoxide, carboxylate, amine, phosphonate, sulfonate or mixtures thereof.
8. Electrocatalytic electrode according to any one of the preceding claims, wherein the mixed oxide is of amorphous structure.
9. Electrocatalytic electrode according to any one of claims 1-8, wherein the mixed oxide consists of a mixture of iron in oxidation state (II) and / or (III) and vanadium in oxidation state (IV) and / or (V).
10. Electrocatalytic electrode according to claim 9, wherein the mixture of iron and vanadium is in a Fe:V molar ratio between 9:1 and 1:9, preferably between 5:1 and 1:
2.
11. Electrocatalytic electrode according to any one of claims 1-8, wherein the mixed oxide including a mixture of iron and vanadium further includes in the mixture at least one metal M selected from the group consisting of: Ti, Cr, Mn, Co, Ni, Cu, Zn, Ga, Ge, Zr, Mo, Ru, Rh, Pd, Ag, In, Sn, W, Re Os, Ir, Pt, Au and Ce.
12. Electrocatalytic electrode according to claim 11, wherein the mixture is ternary and where the iron, vanadium and metal M are in a molar ratio Fe:V:M comprised between 9:0.5:0.5 and 2:5:3, preferably between 4:3:0.5 and 6:5:1.5, more preferably around 5:4:
1.
13. Electrocatalytic electrode according to claim 1, wherein the coating film also includes metal nanoparticles and / or metal oxide nanoparticles other than the metals that form part of the structure of the mixed oxide, said nanoparticles being dispersed in the organic part of the metal-organic matrix.
14. Electrocatalytic electrode according to claim 13, wherein the nanoparticles are formed from salts and / or oxides of a metal selected from the group consisting of: Ti, Cr, Mn, Co, Ni, Cu, Zn, Ga, Ge, Zr, Mo, Ru, Rh, Pd, Ag In, Sn, W, Re, Os, Ir, Pt, Au, and Ce.
15. Electrocatalytic electrode according to claim 14, wherein the nanoparticles are formed from salts and / or oxides of a metal selected from Ni, Au, Ag, Pd, Ru and Ir, preferably Ni, Ru, Pd and Ir.
16. Electrocatalytic electrode according to any one of the preceding claims, wherein, in use, it is electro-catalytically active.
17. Electrocatalytic electrode according to claim 1, wherein the electrically conductive base substrate is made of a material that meets at least one of the following requirements: inorganic, organic, flexible, rigid, semi-rigid, transparent, opaque, solid or porous.
18. Electrocatalytic electrode according to any of claims 1 to 17 obtainable by a wet deposition method.
19. Method for obtaining an electrocatalytic electrode as defined in claims 1 to 18 comprising an electrically conductive base substrate and a coating film on the base substrate, comprising a coating, characterized in that the method comprises the steps of: i-1) preparing a vanadium oxide precursor solution which includes selecting an organic or inorganic counter ion salt of vanadium (II), (III), (IV), and / or (V) and dissolving the vanadium salt in a non-aqueous solvent; i-2) preparing an iron oxide precursor solution which includes selecting an iron (II) and / or (III) salt and dissolving the iron salt in a non-aqueous solvent; (i) mixing the solutions prepared in steps i-1) - i-2) and depositing the mixture of solutions on the substrate by means of a wet deposition method to obtain the coating film; and (iii) carrying out a thermal curing or first curing at a temperature between 20°C and 250°C to dry the coating film, comprising dispersed in the organic part the mixed, non-stoichiometric oxide, which includes the mixture of iron in oxidation state (II) and / or (III) and vanadium in oxidation state (IV) and / or (V).
20. Method according to claim 19, wherein in step iii) the curing or first thermal curing is carried out at a temperature between 20°C and 200°C or lower than the calcination temperature of the organic material that comes from the anions of the iron and / or vanadium salts of step i).
21. Method according to claim 19, wherein in step i-1) the vanadium salt is vanadium (V) and the organic counterion is selected from triisopropoxide oxide, tripropoxide oxide and triethoxide oxide.
22. Method according to claim 19, wherein in step i-1) the solution comprises vanadium salt (II) (III) (IV) and / or (V) at a concentration equal to or greater than 0.05M, preferably a concentration greater than 0.1M and less than 3M.
23. Method according to claim 19, wherein in step i-2) the iron salt (II) and / or (III) is selected from chloride, perchlorate, p-toluenesulfonate, acetate, formate, oxalate, acetylacetonate, tartrate, or citrate.
24. Method according to claim 19, wherein in step i-2) the solution comprises iron (II) and / or (III) salt at a concentration equal to or greater than 0.05M, preferably greater than 0.1M and less than 3M.
25. The method of claim 19, further comprising preparing the mixed oxide comprising a mixture of iron, vanadium and at least one metal M, other than iron and vanadium, selected from the group consisting of Ti, Cr, Mn, Co, Ni, Cu, Zn, Ga, Ge, Zr, Mo, Ru, Rh, Pd, Ag, In, Sn, W, Re, Os, Ir, Pt, Au and Ce, the method further comprising, for each additional metal M added to the mixture of iron and vanadium, repeating: - i-3) , preparing a precursor solution of a metal oxide from one or more salts and / or one or more oxides of the metal M in a non-aqueous solvent to obtain the solution of one or more salts and / or one or more oxides of the metal M, and - in step ¡i), also mix the solution prepared in step i-3).
26. Method according to claim 25, wherein in step i-3) the solution comprises one or more salts and / or one or more oxides of the metal M at a concentration equal to or greater than 0.05M, preferably greater than 0.1M and less than 3M.
27. Process according to any one of claims 19, 25-26, wherein the non-aqueous solvent is independently selected from glycol ethers, glycol ether acetates and derivatives or mixtures thereof.
28. Process according to claim 19, 25-27, wherein the non-aqueous solvent is independently selected from 2-Methoxyethanol, 2-Ethoxyethanol, 2-Butoxyethanol, 2-(2-Ethoxy-ethoxy)ethanol, 2-Propoxyethanol, 2-Isopropoxyethanol, 2-Benzyloxyethanol, 2-(2-Methoxyethoxy)ethanol and 2-(2-Butoxyethoxy)ethanol.
29. Method according to claim 19 and / or 25 which further comprises preparing nanoparticles of metals and / or oxides of metals other than iron and vanadium from a metal selected from the group consisting of: Ti, Cr, Mn, Co, Ni, Cu, Zn, Ga, Ge, Zr, Mo, Ru, Rh, Pd, Ag, In, Sn, W, Re, Os, Ir, Pt, Au, and Ce, where the method further comprises the steps of: - i-4) preparing a solution of one or more metal salts and / or one or more metal oxides from one or more salts and / or one or more oxides of at least one metal selected from the group consisting of Ti, Cr, Mn, Co, Ni, Cu, Zn, Ga, Ge, Zr, Mo, Ru, Rh, Pd, Ag, In, Sn, W, Re, Os, Ir, Pt, Au and Ce in a non-aqueous solvent; and furthermore, in step ¡i), mixing the solution or solutions prepared in step i-4) with the solutions prepared in steps i-1) and i-2), and optionally with the solution or solutions prepared in step i-3); and in step iii), after carrying out the first curing, further carrying out a second curing at a temperature higher than the temperature of the first curing and lower than 350 C to obtain nanoparticles of metals and / or oxides of metals other than iron and vanadium.
30. Method according to claim 29, wherein the temperature of the second curing is higher than the temperature of the first curing and is between a value greater than 100°C and less than 350°C, preferably greater than 200°C and less than 350°C.
31. Use of the electrocatalytic electrode defined in any one of claims 1-18 as an electrocatalytic electrode for the production of molecular hydrogen.
32. Use according to claim 31, wherein the electrocatalytic electrode comprises the coating film with the mixed oxide that includes a mixture of iron and vanadium, and optionally at least one additional metal M, for application as an electrocatalytic electrode in alkaline water electrolysis (AE).
33. Use according to claim 31, wherein the electrocatalytic electrode comprises the coating film with the mixed oxide that includes a mixture of iron and vanadium, and optionally at least one additional metal M, for application as an electrocatalytic electrode in alkaline anion exchange electrolysis (AEM).
34. Use according to claim 31, wherein the electrocatalytic electrode comprises the coating film with the mixed oxide that includes a mixture of iron and vanadium, and optionally at least one additional metal M, for application as a selective electrocatalytic electrode.
35. Use according to claim 31, wherein the electrocatalytic electrode comprises the coating film with the mixed oxide that includes a mixture of iron and vanadium, and optionally at least one additional metal M, for application as an electrocatalytic electrode in the electrolytic oxidation of organic compounds.
36. Use according to claim 35, wherein the organic compounds include derivatives of glycerol and / or lignocellulose.
37. Use of the electrocatalytic electrode according to claim 31 in photocatalysis.
Citation Information
Patent Citations
Electrocatalytic materials and methods for manufacturing same
CN103974769A
Method for producing electrodes having mixed metal oxide catalyst coatings
EP0014596A1
Iron-doped vanadium(v) oxides
EP2220000A1
Preparation method and application of porous iron doped vanadium oxide electrode material
CN108807889A
Cited By
Thermal oxidation nickel-iron-vanadium anode and preparation method thereof
CN121228277A