Lithium ion secondary battery

The lithium ion battery configuration with lithium cobalt oxide and fluorinated carbonates in the electrolyte addresses discharge capacity and temperature range issues, enhancing reliability and safety by minimizing SEI film formation and maintaining high performance across varying temperatures.

WO2024201266A1PCT designated stage expired Publication Date: 2024-10-03SEMICON ENERGY LAB CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2024/052825
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-11
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium ion secondary batteries face challenges in maintaining discharge capacity and cycle characteristics, reliability, safety, and cost, particularly in operating over a wide temperature range without significant deterioration.

Method used

A lithium ion battery configuration featuring a positive electrode active material with lithium cobalt oxide containing magnesium, aluminum, and fluorine, and an electrolyte comprising fluorinated cyclic and chain carbonates, which suppresses the formation of a Solid Electrolyte Interface (SEI) film, allowing for charging and discharging from sub-zero to high temperatures with improved impedance and stability.

Benefits of technology

The solution enables lithium ion batteries to maintain high discharge capacity and reliability over a wide temperature range, reducing deterioration and the need for aging treatments, while ensuring safety and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IB2024052825_03102024_PF_FP_ABST
    Figure IB2024052825_03102024_PF_FP_ABST
Patent Text Reader

Abstract

One aspect of the present invention provides a secondary battery that can be used in a wide temperature range and that is not easily affected by ambient temperatures. Also provided is a highly safe secondary battery. A barrier layer is provided to a positive electrode active material, and an electrolyte that contains a fluorinated cyclic carbonate or a fluorinated chain carbonate is used. As a result of the configuration of the present embodiment, there is substantially no coating film formed on the positive electrode active material surface, and ideally there is no coating film. An aging treatment for forming a coating film on the positive electrode active material can also be eliminated.
Need to check novelty before this filing date? Find Prior Art

Description

Lithium-ion secondary battery

[0001] One aspect of the present invention relates to a lithium-ion secondary battery.

[0002] One embodiment of the present invention is not limited to the above fields, and relates to a semiconductor device, a display device, a light-emitting device, a power storage device, a lighting device, an electronic device, a vehicle, and a manufacturing method thereof. The above-described semiconductor device, display device, light-emitting device, power storage device, lighting device, electronic device, and vehicle can use the lithium-ion secondary battery of one embodiment of the present invention as a necessary power source. For example, the above-described electronic device includes an information terminal device equipped with a lithium-ion secondary battery. Furthermore, the above-described power storage device includes a stationary power storage device.

[0003] A lithium-ion secondary battery (sometimes referred to as a lithium-ion battery) is a battery that uses lithium ions as the carrier ion. Lithium-ion batteries are secondary batteries that can be used repeatedly by charging and discharging.

[0004] In recent years, there has been active development of various types of energy storage devices, such as lithium-ion secondary batteries, lithium-ion capacitors, air batteries, and all-solid-state batteries. Demand for high-power, high-capacity lithium-ion secondary batteries has expanded rapidly in line with the development of the semiconductor industry, and they have become indispensable in today's information society as a rechargeable energy source.

[0005] In particular, there is a high demand for secondary batteries with a large discharge capacity per weight and excellent cycle characteristics for mobile electronic devices, etc. To meet this demand, improvements to the positive electrode active materials of the positive electrodes of secondary batteries have been actively pursued (e.g., Patent Documents 1 to 3).

[0006] Lithium-ion batteries are also expected to be able to charge and discharge over a wide temperature range depending on the application. Therefore, research and development into enabling lithium-ion batteries to be charged and discharged at high and low temperatures is actively underway. Non-Patent Document 1 proposes an electrolyte containing methyl 3,3,3-trifluoropropionate (MTFP):fluoroethylene carbonate (FEC) in a 9:1 ratio to improve output characteristics below freezing. Non-Patent Document 2 reports the crystal structure of a positive electrode active material.

[0007] JP 2019-179758 A WO2020 / 026078 Pamphlet JP 2022-070247 A

[0008] John, H. et al. , “An All-Fluorinated Ester Electrolyte for Stable High-Voltage Li Metal Batteries Capable of Ultra-Low-Temperature Operation”, ACE Energy LETTERS, 2020, 5, 1438-1447 Zhaohui Chen et al. , “Staging Phase Transitions in LixCoO▲2▼”, Journal of The Electrochemical Society, 2002, 149 (12) A1604-A1609

[0009] Lithium ion secondary batteries still have room for improvement in various aspects, such as discharge capacity, cycle characteristics, reliability, safety, and cost.

[0010] An object of one embodiment of the present invention is to provide a secondary battery in which a decrease in charge / discharge capacity during charge / discharge cycles is suppressed. Another object is to provide a secondary battery that has a large charge / discharge capacity and is safe or highly reliable. Another object is to provide a positive electrode active material or composite oxide that can be used in a lithium ion secondary battery and in which a decrease in discharge capacity during charge / discharge cycles is suppressed. Another object is to provide a positive electrode active material or composite oxide whose crystal structure is not easily destroyed even after repeated charge / discharge. Another object is to provide a positive electrode active material or composite oxide that has a large charge / discharge capacity.

[0011] Another object of one embodiment of the present invention is to provide a positive electrode active material, a composite oxide, a power storage device, or a manufacturing method thereof.

[0012] Another object of one embodiment of the present invention is to provide a lithium-ion battery including an electrolyte containing a new organic solvent and a new positive electrode active material, which enables charging and discharging in a wide temperature range including temperatures below freezing to high temperatures.

[0013] One aspect of the present invention is a lithium-ion secondary battery including a positive electrode having a positive electrode active material and an electrolyte, wherein the positive electrode active material includes lithium cobalt oxide containing magnesium, the magnesium concentration in a surface layer portion of the positive electrode active material is higher than the magnesium concentration inside the positive electrode active material, and the electrolyte includes a fluorinated cyclic carbonate and a fluorinated chain carbonate.

[0014] In the above-described configuration, the positive electrode active material is lithium cobalt oxide further containing aluminum, nickel, and fluorine.

[0015] In addition, in the above configuration, when AC impedance is measured after charging the lithium ion secondary battery to a voltage of 4.5 V, the impedance value satisfies the requirement of less than 90 mΩ at a frequency of 1 kHz.

[0016] In one embodiment of the present invention, an additive is not mixed into an organic solvent for forming a coating (solid electrolyte interface: SEI film) at the interface between an electrode (active material layer) and an electrolyte. In particular, vinylene carbonate (VC) adversely affects the positive electrode and causes deterioration, so the electrolyte used in the battery of one embodiment of the present invention preferably does not contain VC.

[0017] Therefore, one of the characteristics of the positive electrode active material, lithium cobalt oxide, is that it has almost no coating on its surface and is in contact with the electrolyte.

[0018] In this specification, the term "positive electrode active material" refers to a compound containing a transition metal and oxygen, capable of inserting and desorbing carrier ions. Compounds containing oxygen are sometimes called oxides or composite oxides. Lithium ions are typically used as carrier ions, but sodium ions, magnesium ions, or the like may also be used. Carbonates and hydroxyl groups adsorbed after the preparation of the positive electrode active material are not included in the positive electrode active material. Furthermore, electrolytes, organic solvents, binders, conductive materials, or compounds derived from these materials attached to the positive electrode active material are also not included in the positive electrode active material.

[0019] In this specification, "below freezing" refers to 0° C. or below, "high temperature" refers to 25° C. or above, and room temperature refers to a temperature higher than 0° C. but lower than 25° C. In this specification, "a temperature range higher than 0° C. and including high temperatures" includes the above-mentioned room temperature.

[0020] In this specification and the like, the term "particle" used in reference to active material particles and the like is not limited to referring only to spherical shapes (circular cross-sectional shapes). For example, particles may have cross-sectional shapes such as elliptical and asymmetric shapes, and further, the individual particles do not need to be uniform and may have irregular shapes.

[0021] A "nonaqueous electrolyte" refers to a liquid electrolyte containing an organic solvent exhibiting carrier ion conductivity, but is not limited to a liquid state in the present invention. Therefore, in this specification, the concept of a nonaqueous electrolyte is referred to as an "electrolyte." That is, the electrolyte of one embodiment of the present invention is not limited in any way to its state, and includes, for example, an electrolyte whose viscosity has increased from a liquid state as a result of viscosity adjustment. Furthermore, the electrolyte also includes a solid or semi-solid state. A semi-solid state refers to a state intermediate between a liquid and a solid state. Specific examples of semi-solid states include flexible solids, typically gels. Semi-solid electrolytes are generally referred to as semi-solid electrolytes, and the electrolyte of one embodiment of the present invention also includes a semi-solid electrolyte. The liquid, solid, or semi-solid state, or viscosity, is determined when the lithium-ion battery is placed at 25°C.

[0022] In this specification and the like, a value that indicates the magnitude of viscosity is called viscosity, and "appropriate viscosity" means that the viscosity is appropriate for a lithium ion battery.

[0023] In this specification and the like, segregation of a certain element refers to a state in which a certain element (for example, A) is distributed non-uniformly in a solid composed of a plurality of elements (for example, A, B, C).

[0024] In this specification, the distribution of a certain element refers to the spread of locations where the element is continuously present when the element is detected within a range that is not noise using any analytical method. The continuous change in the concentration of the element is sometimes called a concentration gradient. The maximum value in the distribution is sometimes called a peak. When identifying a peak, it is possible to target a distribution limited to a certain region. The above-mentioned distribution is not limited to a normal distribution. When the distribution corresponds to a normal distribution, the half-width of the distribution can also be determined.

[0025] In this specification, uneven distribution refers to the concentration of an element in a certain region being different from that in other regions. This is synonymous with uneven distribution or the presence of a mixture of high-concentration and low-concentration regions. Uneven distribution through solid solution is called segregation.

[0026] By providing a barrier layer on the positive electrode active material and using an electrolyte containing a fluorinated cyclic carbonate or a fluorinated chain carbonate in the configuration of this embodiment, almost no coating is formed on the surface of the positive electrode active material, and ideally, no coating is formed on the surface.

[0027] One aspect of the present invention allows charging and discharging over a wide temperature range, including from below freezing to high temperatures.

[0028] According to one embodiment of the present invention, deterioration of a secondary battery can be suppressed and reliability can be improved.

[0029] Furthermore, it is possible to eliminate the need for an aging treatment for forming a coating on the positive electrode active material. The aging treatment is sometimes called initial charge / discharge or conditioning.

[0030] Note that the above-described effects do not preclude the existence of other effects. Furthermore, the above-described effects are considered to be independent of each other, and one embodiment of the present invention does not necessarily exhibit all of the above-described effects. Furthermore, effects other than those described above can be extracted from the description of this specification and the like.

[0031] FIGS. 1A and 1B are diagrams illustrating a lithium-ion battery of one embodiment of the present invention. FIGS. 2A to 2C are diagrams illustrating a manufacturing method of a positive electrode active material of one embodiment of the present invention. FIGS. 3A to 3F are diagrams illustrating a positive electrode active material of one embodiment of the present invention. FIG. 4 is a diagram illustrating a crystal structure of a positive electrode active material of one embodiment of the present invention. FIG. 5 is a diagram illustrating a crystal structure of a positive electrode active material. FIG. 6 is a diagram illustrating diffraction peaks of a positive electrode active material. FIG. 7 is a diagram illustrating diffraction peaks of a positive electrode active material. FIGS. 8A and 8B are diagrams illustrating diffraction peaks of a positive electrode active material. FIGS. 9A to 9D are diagrams illustrating a positive electrode of one embodiment of the present invention. FIGS. 10A and 10B are diagrams illustrating a lithium-ion battery of one embodiment of the present invention. FIGS. 11A to 11C are diagrams illustrating a lithium-ion battery of one embodiment of the present invention. FIGS. 12A to 12D are diagrams illustrating a lithium-ion battery and a power storage system of one embodiment of the present invention. FIGS. 13A to 13C are diagrams illustrating a lithium-ion battery of one embodiment of the present invention. FIGS. 14A to 14C are diagrams illustrating a lithium-ion battery of one embodiment of the present invention. FIGS. 15A to 15C are diagrams illustrating an electric vehicle of one embodiment of the present invention. FIGS. 16A to 16D are diagrams illustrating a transportation vehicle of one embodiment of the present invention. FIGS. 17A to 17C are diagrams illustrating a motorcycle or the like of one embodiment of the present invention. FIGS. 18A to 18D are diagrams illustrating an electronic device or the like of one embodiment of the present invention. FIGS. 19A to 19D are diagrams illustrating an example of space equipment. FIG. 20A is a graph showing the cycle characteristics of Sample 1 having an electrolyte and a positive electrode active material of one embodiment of the present invention at 25° C. and an end voltage of 4.7 V. FIG. 20B is a graph showing the cycle characteristics of Sample 1 having an electrolyte and a positive electrode active material of one embodiment of the present invention at 45° C. and an end voltage of 4.7 V. FIG. 21 is a graph showing the cycle characteristics of Sample 1 having an electrolyte and a positive electrode active material of one embodiment of the present invention at an end voltage of 4.8 V. FIG. 22 is a graph showing the charge / discharge characteristics of Sample 1. Fig. 23A is a graph of Sample 1 with the vertical axis representing capacity and the horizontal axis representing the number of cycles, and Fig. 23B is a graph of Sample 1 with the vertical axis representing charge / discharge efficiency and the horizontal axis representing the number of cycles. Figs. 24A and 24B are diagrams illustrating AC impedance measurement. Figs. 25A to 25C are diagrams illustrating the results of AC impedance measurement of Sample 1_P.

[0032] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be readily understood by those skilled in the art that various modifications can be made to the embodiments and details. Furthermore, the present invention should not be interpreted as being limited to the description of the embodiments shown below.

[0033] Embodiment 1 In this embodiment, a lithium-ion battery which is one embodiment of the present invention will be described with reference to the drawings.

[0034] <Lithium-ion battery> A lithium-ion battery according to one embodiment of the present invention has an electrolyte that allows charging and discharging over a wide temperature range, including at least sub-zero temperatures and even high temperatures. In addition to the electrolyte, the lithium-ion battery includes a negative electrode, a positive electrode, a separator between the negative electrode and the positive electrode, and an exterior covering the negative electrode and the positive electrode. Depending on the shape of the exterior, the battery is called a laminated lithium-ion battery, a coin-cell lithium-ion battery, or a cylindrical lithium-ion battery, but the present invention is not limited to the shape of the exterior. The separator can be omitted if the electrolyte is solid or semi-solid.

[0035] 1A illustrates an example of the configuration of a lithium ion battery 100. In a cross-sectional view, the lithium ion battery 100 has a negative electrode 106, a separator 108, and a positive electrode 107. In the lithium ion battery 100, the electrolyte 109 is in a liquid state, and the electrolyte 109 is present throughout the negative electrode 106, the separator 108, and the positive electrode 107. As described above, the electrolyte 109 is not limited to being in a liquid state.

[0036] The negative electrode 106 includes a negative electrode current collector 101 and a negative electrode active material layer 102. The negative electrode active material layer 102 contains at least an active material and may contain a conductive material and / or a binder. A known material can be used for the negative electrode active material, and details of the material will be described later. The positive electrode 107 includes a positive electrode current collector 105 and a positive electrode active material layer 104. The positive electrode active material layer 104 contains at least an active material and may contain a conductive material and / or a binder. Although a known material may be used for the positive electrode active material, the use of a positive electrode active material of one embodiment of the present invention allows the battery to withstand high-voltage charging and increase the discharge capacity of a lithium-ion battery. The positive electrode active material of one embodiment of the present invention will be described later.

[0037] The conductive material has the function of assisting the current path between active materials and / or between the active material and the current collector. Known materials can be used as the conductive material, and details will be described later. The binder, also called a binding agent, has the function of assisting the adhesion between active materials and / or between the active material and the current collector. Known materials can be used as the binder, and details will be described later.

[0038] 1B illustrates a lithium ion battery 100 that does not have the negative electrode active material layer 102, unlike the lithium ion battery 100 in FIG. 1A. The negative electrode active material layer 102 can be eliminated depending on the material of the negative electrode current collector 101. The other configurations of the lithium ion battery 100 in FIG. 1B are the same as those of the lithium ion battery 100 in FIG. 1A, and therefore will not be described again.

[0039] In this embodiment, a lithium ion battery having excellent discharge characteristics and / or excellent charge characteristics can be realized over a wide temperature range, including temperatures from below freezing to high temperatures. The following description focuses on the configuration of the lithium ion battery required for this purpose. Specifically, the description focuses on the positive electrode active material and electrolyte. Details of the configuration of the lithium ion battery other than the positive electrode active material and electrolyte will be described in the third and subsequent embodiments.

[0040] <Positive Electrode Active Material> The positive electrode active material has the function of incorporating and / or releasing lithium ions, which are carrier ions, during charging and discharging. The positive electrode active material used in one embodiment of the present invention enables charging and discharging even at high charging voltages (hereinafter also referred to as "high charging voltages") over a wide temperature range from below freezing to high temperatures, and can be made of a material that undergoes little deterioration (or little increase in resistance) during charging and discharging. Unless otherwise specified in this specification, the "charging voltage" is expressed relative to the potential of lithium metal. Furthermore, in this specification, the "high charging voltage" refers to a charging voltage of, for example, 4.5 V or higher, preferably 4.6 V or higher, and more preferably 4.65 V or higher.

[0041] The positive electrode active material is not limited to one type, and two or more materials with different median diameters (D50) may be mixed, or two or more materials with different compositions may be mixed, as long as they are materials that undergo little deterioration during charge and discharge even at high charge voltages over a wide temperature range, including from below freezing to high temperatures. In this specification, etc., "different compositions" includes not only cases where the composition of elements contained in the materials is different, but also cases where the ratios of elements contained in the materials are different even if the composition of elements contained in the materials is the same.

[0042] As mentioned above, in this specification, a "high charging voltage" is defined as 4.5 V or higher based on the potential when the negative electrode is made of lithium metal, but when the potential when the negative electrode is made of a carbon material (e.g., graphite) is used as the reference, a "high charging voltage" is defined as 4.4 V or higher. In short, in the case of a half cell using lithium metal as the negative electrode, a charging voltage of 4.5 V or higher is defined as a high charging voltage, and in the case of a full cell using a carbon material (e.g., graphite) as the negative electrode, a charging voltage of 4.4 V or higher is defined as a high charging voltage.

[0043] The temperature during charging or discharging described in this specification refers to the temperature of the environment in which the lithium-ion battery is placed (hereinafter, sometimes referred to as "environmental temperature" in this specification). In measuring battery characteristics, a thermostatic chamber stabilized at a desired temperature is used, so the environmental temperature is equal to the temperature of the thermostatic chamber. After placing a test cell (e.g., a full cell or a half cell) to be measured in the thermostatic chamber, measurement can be started after a sufficient time (e.g., one hour or more) has elapsed until the test cell reaches the same temperature as the thermostatic chamber, but measurement of battery characteristics is not necessarily limited to this method.

[0044] <Electrolyte> As the electrolyte used in one embodiment of the present invention, a material having excellent lithium ion conductivity over a wide temperature range including from below freezing to high temperatures can be used.

[0045] The electrolyte contains an organic solvent, but the organic solvent of the electrolyte according to one embodiment of the present invention is not limited to being liquid at 25° C., and may be solid at 25° C. or semi-solid at room temperature. Note that the organic solvent of the electrolyte according to one embodiment of the present invention is preferably liquid over a wide temperature range, including temperatures from below freezing to high temperatures, but is not limited thereto. The organic solvent may be liquid, solid, or semi-solid over a wide temperature range, including temperatures from below freezing to high temperatures.

[0046] <Organic Solvent> The organic solvent described in this embodiment may contain a fluorinated cyclic carbonate (sometimes referred to as a fluorinated cyclic carbonate) or a fluorinated chain carbonate (sometimes referred to as a fluorinated chain carbonate). Furthermore, the organic solvent preferably contains both a fluorinated cyclic carbonate and a fluorinated chain carbonate. Both the fluorinated cyclic carbonate and the fluorinated chain carbonate have electron-withdrawing substituents, and have lower solvation energy of lithium ions than organic compounds without electron-withdrawing substituents. Therefore, both the fluorinated cyclic carbonate and the fluorinated chain carbonate are suitable organic solvents.

[0047] Examples of fluorinated cyclic carbonates that can be used include fluoroethylene carbonate (fluorinated ethylene carbonate, fluoroethylene carbonate, FEC, F1EC), difluoroethylene carbonate (DFEC, F2EC), trifluoroethylene carbonate (F3EC), and tetrafluoroethylene carbonate (F4EC). DFEC includes isomers such as cis-4,5 and trans-4,5. Since all of these fluorinated cyclic carbonates have electron-withdrawing substituents, they are believed to have low solvation energies for lithium ions.

[0048] The following structural formula (H10) is the structural formula of FEC: In FEC, the electron-withdrawing substituent is an F group.

[0049]

[0050] Methyl 3,3,3-trifluoropropionate is an example of a fluorinated chain carbonate. The following structural formula (H22) is the structural formula of methyl 3,3,3-trifluoropropionate. The abbreviation for methyl 3,3,3-trifluoropropionate is "MTFP." In MTFP, the electron-withdrawing substituent is CF 3 It is the base.

[0051]

[0052] An example of a fluorinated chain carbonate is trifluoromethyl 3,3,3-trifluoropropionate. The following structural formula (H23) is the structural formula of trifluoromethyl 3,3,3-trifluoropropionate. The electron-withdrawing substituent is CF 3 It is the base.

[0053]

[0054] An example of a fluorinated chain carbonate is trifluoromethyl propionate. The following structural formula (H24) is the structural formula of trifluoromethyl propionate. The electron-withdrawing substituent is CF 3 It is the base.

[0055]

[0056] An example of a fluorinated chain carbonate is methyl 2,2-difluoropropionate. The following structural formula (H25) is the structural formula of methyl 2,2-difluoropropionate. The electron-withdrawing substituent is CF 2 It is the base.

[0057]

[0058] The organic solvent of the electrolyte according to one embodiment of the present invention may contain two or more selected from the fluorinated cyclic carbonates and the fluorinated chain carbonates. For example, the organic solvent described in this embodiment may contain FEC and MTFP. The reason for this will be described below.

[0059] <FEC and MTFP> FEC is a cyclic carbonate with a high dielectric constant, and therefore, when used in an organic solvent, it has the effect of promoting the dissociation of lithium salts. Since FEC has a lower solvation energy than ethylene carbonate (abbreviated as "EC"), which does not have electron-withdrawing substituents, it can be said that the bond between lithium ions and the solvent is easily separated. Furthermore, FEC has a deep HOMO, and a deep HOMO makes it less susceptible to oxidation, improving oxidation resistance. On the other hand, FEC has a high viscosity, and when used alone as an organic solvent, it is difficult to use below freezing. Therefore, the organic solvent specifically described as one embodiment of the present invention further includes MTFP in addition to FEC. MTFP is a chain carbonate and has the effect of reducing or maintaining the viscosity of the entire electrolyte. Of course, MTFP also has a lower solvation energy than methyl propionate (abbreviated as "MP"), which does not have electron-withdrawing substituents, and therefore the bond between lithium ions and the solvent is easily separated.

[0060] FEC and MTFP having such physical properties can be mixed and used in a volume ratio of x:100-x (where 5≦x≦30, preferably 10≦x≦20), where the total amount of these two organic solvents is 100%. It is preferable to mix the organic solvents so that there is more MTFP than FEC. The volume ratio may be the volume ratio measured before mixing the organic solvents, and the outside air may be room temperature (typically 25°C) when mixing the organic solvents. An organic solvent mixed with FEC and MTFP is preferred because it exhibits a viscosity that allows operation as a lithium-ion battery and maintains an appropriate viscosity over a wide temperature range, including from below freezing to high temperatures.

[0061] Because typical organic solvents used in lithium ion batteries freeze at around −20° C., it is difficult to fabricate a lithium ion battery that can be charged and discharged at −40° C., preferably −50° C. The organic solvent described as an example in this embodiment allows the freezing point to be −40° C. or lower, preferably −50° C. or lower, thereby realizing a lithium ion battery that can be charged and discharged even in a sub-zero environment of −40° C. or lower. As a result, a lithium ion battery that can be charged and discharged over a wide temperature range, including at least sub-zero temperatures, can be realized.

[0062] While FEC has been described as a representative example above, any of the organic compounds described as fluorinated cyclic carbonates can be said to have the effect of promoting dissociation of lithium salts, have low solvation energy, making it easy for the bonds between lithium ions and the solvent to separate, and have high viscosity, making them difficult to use at sub-zero temperatures when used alone. Furthermore, although MTFP has been described as a representative example above, any of the organic compounds described as fluorinated chain carbonates can be said to have the effect of reducing or maintaining the viscosity of the electrolyte. Therefore, as long as the organic solvent according to one embodiment of the present invention contains a fluorinated cyclic carbonate and a fluorinated chain carbonate, it is possible to provide a lithium-ion battery that can be charged and discharged over a wide temperature range, including at least temperatures below freezing.

[0063] The organic solvent described above is free from granular dust or molecules other than the constituent molecules of the organic solvent (hereinafter simply referred to as "impurities"), and oxygen (O 2), water (H 2 It is preferable that the organic solvent has a low content of impurities (O or water) and is highly purified. Specifically, the amount of the impurities contained in the organic solvent is 100 ppm or less, preferably 50 ppm or less, and more preferably less than 10 ppm.

[0064] In order to reduce the amount of impurities contained in the organic solvent to less than 10 ppm, it is preferable to heat the organic solvent under reduced pressure before use in a secondary battery to remove the impurities. When using the organic solvent in a secondary battery, the organic solvent is injected in a dry room where the moisture content is sufficiently reduced, and the secondary battery is manufactured.

[0065] For example, water can be detected by Karl Fischer titration, and water with different binding strengths (e.g., crystal water, combined water, or adherent water) can be quantified by changing the heating conditions. For example, under heating conditions of 120°C for 30 minutes, water generated at around 100°C can be mainly detected. In this specification, the unit ppm for the amount of impurities contained in the organic solvent refers to mass fraction, i.e., ppm (mass / mass).

[0066] During charge and discharge of the secondary battery, a part of the organic solvent is decomposed, which reduces the reliability of the secondary battery. 2 ), water (H 2 Since there is a risk that the organic solvent may be decomposed due to impurities such as fluorine (O) or water, the decomposition of the organic solvent can be suppressed by containing fewer impurities in the organic solvent, as described above. Furthermore, if fluorine is present at a site likely to be the starting point of decomposition in the molecule of a material used in the organic solvent, decomposition is less likely to occur, and therefore it is preferable to use such a material.

[0067] <Lithium Salt> The lithium salt dissolved in the organic solvent is, for example, LiPF 6 , LiClO 4 , LiAsF 6 , LiBF 4 , LiAlCl 4 , LiSCN, LiBr, LiI, Li 2 SO 4 , Li 2 B 10 Cl10 , Li 2 B 12 Cl 12 , LiCF 3 SO 3 , LiC 4 F 9 SO 3 , LiC(CF 3 SO 2 ) 3 , LiC(C 2 F 5 SO 2 ) 3 , LiN(CF 3 SO 2 ) 2 , LiN(C 4 F 9 SO 2 ) (CF 3 SO 2 ), LiN(C 2 F 5 SO 2 ) 2 , or lithium bis(oxalato)borate (LiBOB), and the lithium salts may be used in any combination and in any ratio. The lithium salt is one of the components included in the electrolyte of one embodiment of the present invention, but is not necessarily included.

[0068] The lithium-ion battery according to one embodiment of the present invention includes at least the above-described positive electrode active material and an electrolyte, and thereby can maintain a state in which no coating or almost no coating is present on the surface of the positive electrode active material, and can be charged and discharged over a wide temperature range, including from below freezing to high temperatures.

[0069] Embodiment 2 In this embodiment, a positive electrode active material that can be used in a lithium-ion battery according to one embodiment of the present invention (hereinafter also referred to as a "positive electrode active material that can be used as one embodiment of the present invention") and a manufacturing method thereof will be described with reference to FIGS.

[0070] As described above in Embodiment 1, any material that undergoes little deterioration due to charge and discharge at a high charge voltage can be used as the positive electrode active material that can be used in the lithium-ion battery of one embodiment of the present invention. Therefore, the positive electrode active material that can be used in the lithium-ion battery disclosed in this specification and the like does not need to be interpreted as being limited to the specific materials described in this embodiment and the like. Materials that are known as materials that undergo little deterioration due to charge and discharge even at a high charge voltage (for example, 4.5 V or higher) at the time of filing the present application can also be used.

[0071] An example of a method for producing a cathode active material that can be used as one embodiment of the present invention will be described below. In this embodiment, a case where a cathode active material is produced using a solid-phase method will be described. However, a cathode active material produced using a coprecipitation method, a hydrothermal method, or the like, other than the solid-phase method, can also be applied to the lithium-ion battery of the present invention. Note that the flow used to explain the production method and the like in this embodiment indicates the order of elements connected by lines, and does not indicate the order of elements not connected by lines.

[0072] [Method for Producing Positive Electrode Active Material] An example of a flow for producing the positive electrode active material 10 will be described with reference to FIGS. 2A to 2C.

[0073] In step S11 shown in FIG. 2A, a lithium source (Li source) and a transition metal M source (M source) are prepared as starting materials for lithium and transition metal M, respectively.

[0074] As the lithium source, it is preferable to use a compound containing lithium, such as lithium carbonate, lithium hydroxide, lithium nitrate, or lithium fluoride. It is preferable that the lithium source has high purity, and it is preferable to use a material with a purity of, for example, 99.99% or higher.

[0075] The transition metal M may be, for example, one or more of manganese, cobalt, and nickel. When lithium cobalt oxide (LCO) is prepared as the positive electrode active material, cobalt is used as the transition metal M. When nickel-cobalt-manganese composite oxide (NCM) is prepared as the positive electrode active material, cobalt, manganese, and nickel are used as the transition metal M. Aluminum may also be used in addition to the transition metal M.

[0076] As the transition metal M source, it is preferable to use a compound containing the transition metal M, and for example, an oxide or hydroxide of a metal exemplified as the transition metal M can be used. As a cobalt source, cobalt oxide, cobalt hydroxide, etc. can be used. As a manganese source, manganese oxide, manganese hydroxide, etc. can be used. As a nickel source, nickel oxide, nickel hydroxide, etc. can be used. As an aluminum source, aluminum oxide, aluminum hydroxide, etc. can be used. Furthermore, when two or more transition metal M sources are used, it is preferable to prepare the two or more transition metal M sources in a ratio (mixing ratio) that allows the two or more transition metal M sources to form a layered rock salt type crystal structure.

[0077] <Step S12> Next, in step S12 shown in FIG. 2A , the lithium source and the cobalt source are pulverized and mixed to prepare a mixed material. The pulverization and mixing can be performed by either a dry or wet method. The wet method is preferred because it allows for smaller pulverization. When using the wet method, a solvent is prepared. Examples of solvents that can be used include ketones such as acetone, alcohols such as ethanol and isopropanol, ether, dioxane, acetonitrile, and N-methyl-2-pyrrolidone (NMP). It is more preferable to use an aprotic solvent that is less likely to react with lithium. In this embodiment, dehydrated acetone with a purity of 99.5% or higher is used. It is preferable to mix the lithium source and the cobalt source with dehydrated acetone with a purity of 99.5% or higher, with a water content reduced to 10 ppm or less, and then pulverize and mix them. Using dehydrated acetone with the above purity can reduce potential impurities.

[0078] A ball mill, a bead mill, or the like can be used as a means for pulverizing and mixing. When using a ball mill, aluminum oxide balls or zirconium oxide balls are used as pulverizing media. Zirconium oxide balls are preferred because they emit less impurities. Furthermore, when using a ball mill, a bead mill, or the like, it is preferable to set the peripheral speed to 100 mm / s or more and 2000 mm / s or less in order to suppress contamination from the media. In this embodiment, the peripheral speed is set to 838 mm / s (rotation speed 400 rpm, ball mill diameter 40 mm).

[0079] <Step S13> Next, in step S13 shown in FIG. 2A , the mixed material is heated. Heating is preferably performed at a temperature of 800°C to 1100°C, more preferably 900°C to 1000°C, and even more preferably about 950°C. If the temperature is too low, decomposition and melting of the Li source and M source may be insufficient. On the other hand, if the temperature is too high, lithium may sublimate from the Li source and / or the transition metal used as the M source may be excessively reduced. If the heating time is too short, a composite oxide containing lithium and the transition metal M may not be synthesized, but if it is too long, productivity may decrease. Therefore, the heating time is set to 1 hour to 100 hours, and preferably 2 hours to 20 hours. The temperature rise rate depends on the heating temperature reached, but is preferably 80°C / h to 250°C / h, more preferably 100°C / h to 250°C / h.

[0080] The heating atmosphere is preferably an atmosphere with little water. The low water atmosphere can be defined by the dew point, and for example, an atmosphere with a dew point of -50°C or less, more preferably an atmosphere with a dew point of -80°C or less, is considered to be the heating atmosphere. Furthermore, an atmosphere containing oxygen, such as dry air, is preferred as the heating atmosphere. For example, there is a method in which oxygen is continuously introduced into the reaction chamber. In this case, the flow rate of oxygen is preferably 5 L / min or more and 15 L / min or less. The state in which oxygen is continuously introduced into the reaction chamber and flows through the reaction chamber is called "flow."

[0081] In addition to the above-described flow, the heating atmosphere may be changed to an oxygen-containing atmosphere by, for example, reducing the pressure in the reaction chamber, introducing oxygen, and then controlling the oxygen so that it does not enter or leave the reaction chamber. This is called "purging." For example, the reaction chamber may be reduced in pressure to -970 hPa, and then oxygen may be introduced to 50 hPa, and the oxygen entry and exit may be stopped. This state may be referred to as filling the reaction chamber with oxygen.

[0082] Cooling after heating may be carried out by natural cooling, but it is preferable that the temperature drop time from the specified temperature to room temperature is within 10 hours or more and 50 hours or less, for example, 80° C. / h or more and 250° C. / h or less is preferable, and 180° C. / h or more and 210° C. / h or less is more preferable. However, cooling to room temperature is not necessarily required, as long as it is cooled to a temperature acceptable for the next step.

[0083] The heating in this step may be carried out using a rotary kiln or a roller hearth kiln. Heating in a rotary kiln can be carried out while stirring, whether in a continuous or batch system.

[0084] The crucible used for heating is preferably an aluminum oxide crucible. Aluminum oxide crucibles are made of a material that does not easily release impurities. In this embodiment, an aluminum oxide crucible with a purity of 99.9% is used. It is preferable to heat the crucible with a lid. This can prevent the material from volatilizing or sublimating. The lid only needs to prevent the material from volatilizing or sublimating from the time the temperature is increased to the time the temperature is decreased in this step, and the crucible does not necessarily have to be sealed with a lid. For example, as described above, by filling the reaction chamber with oxygen, this step can be performed without sealing the crucible.

[0085] In addition, it is preferable to use a used crucible rather than a new one. In this specification, a new crucible refers to one that has undergone the process of heating a material containing lithium, a transition metal M, and / or an additive element two or less times. A used crucible refers to one that has undergone the process of heating a material containing lithium, a transition metal M, and / or an additive element three or more times. This is because when a new crucible is used, there is a risk that some of the materials, including lithium fluoride, may be absorbed, diffused, migrated, and / or adhered to the sheath during heating. If some of the materials are lost as a result of this, there is a growing concern that the distribution of elements, particularly in the surface layer of the positive electrode active material, may not fall within a desirable range. On the other hand, this risk is less likely with a used crucible.

[0086] After heating, the material may be crushed and sieved as necessary. When recovering the heated material, it may be transferred from the crucible to a mortar and then recovered. It is preferable to use an aluminum oxide mortar or a zirconium oxide mortar. An aluminum oxide mortar is a material that does not easily release impurities. Specifically, an aluminum oxide mortar with a purity of 90% or more, preferably 99% or more, is used. Heating conditions equivalent to those of step S13 can also be applied to heating steps other than step S13, which will be described later.

[0087] <Step S14> By the above steps, a composite oxide containing lithium and a transition metal M (LiMO) is obtained in step S14 of FIG. 2A. 2 The composite oxide can be obtained by 2 However, the composition is not strictly limited to Li:M:O=1:1:2. When cobalt is used as the transition metal M, it is called a composite oxide containing cobalt, and LiCoO 2 However, the composition is not strictly limited to Li:Co:O=1:1:2.

[0088] Although the example of producing the composite oxide by the solid phase method as in steps S11 to S14 has been shown, the composite oxide may also be produced by a coprecipitation method or a hydrothermal method.

[0089] <Step S15> Next, in step S15 shown in FIG. 2A , the composite oxide is heated. Because this is the first heating of the composite oxide, the heating in step S15 is sometimes referred to as initial heating. Alternatively, because it is heating performed before step S20 described below, it is sometimes referred to as preheating or pretreatment. The crucible and / or lid used in this step are the same as those used in step S13. Although the following effects are expected from the initial heating, initial heating is not essential for obtaining a positive electrode active material that is one embodiment of the present invention.

[0090] The initial heating may cause lithium to be released from a portion of the composite oxide. It is also expected to have the effect of increasing the crystallinity of the composite oxide. Furthermore, although the Li source and / or metal M source prepared in step S11 may contain impurities, the initial heating can reduce the amount of impurities in the composite oxide.

[0091] Furthermore, initial heating has the effect of smoothing the surface of the composite oxide. A smooth surface means that there are few irregularities, the surface of the composite oxide is rounded overall, and the corners are also rounded. A surface with little foreign matter adhering to it is also sometimes called smooth.

[0092] For this initial heating, it is not necessary to prepare a raw material such as a Li source, or a material that functions as a flux (a material added to facilitate melting).

[0093] If the heating time in this step is too short, sufficient effects will not be obtained, but if it is too long, productivity will decrease. For example, the heating conditions can be selected from those described in step S13. Regarding the heating conditions, the heating temperature in this step is preferably lower than the temperature in step S13 in order to maintain the crystalline structure of the complex oxide. Furthermore, the heating time in this step is, for example, at a temperature of 700°C or higher and 1000°C or lower for 2 hours or longer and 20 hours or shorter in order to maintain the crystalline structure of the complex oxide.

[0094] The effect of increasing the crystallinity of the composite oxide also includes, for example, the effect of alleviating distortion resulting from differential shrinkage caused by heating the composite oxide, and the effect of alleviating deviation resulting from the differential shrinkage.

[0095] The heating in step S13 may cause a temperature difference between the surface and the interior of the composite oxide. The temperature difference may induce a contraction difference. It is also thought that the temperature difference causes a difference in fluidity between the surface and the interior, resulting in a contraction difference. The energy associated with the contraction difference causes a difference in internal stress in the composite oxide, which causes distortion. This energy is sometimes called strain energy. The internal stress is removed by the initial heating in step S15; in other words, the strain energy is thought to be reduced by the initial heating in step S15. When the strain energy is reduced, the distortion of the composite oxide is alleviated. Therefore, the surface of the composite oxide may become smoother after step S15. In other words, it is thought that the contraction difference that occurred in the composite oxide is alleviated after step S15, resulting in a smoother surface of the composite oxide. Step S15 is sometimes called tempering or annealing the composite oxide.

[0096] Furthermore, the difference in shrinkage may cause microscopic deviations in the composite oxide, for example deviations in the crystal plane. It is preferable to carry out this step in order to reduce such deviations. By going through this step, it is possible to reduce the deviations in the composite oxide. If the deviations are made uniform, the surface of the composite oxide may become smooth. This is also referred to as the alignment of crystal grains. In other words, it is believed that by going through step S15, deviations in the crystals and the like that have occurred in the composite oxide are alleviated, and the surface of the composite oxide becomes smooth.

[0097] The smooth surface of a composite oxide can be said to have a surface roughness of at least 10 nm or less when surface irregularity information is quantified from measurement data at a cross section of the composite oxide. The cross section is, for example, a cross section obtained when observing with a scanning transmission electron microscope (referred to as STEM).

[0098] When a composite oxide with a smooth surface is used as a positive electrode active material, deterioration during charging and discharging of a lithium ion battery is reduced and cracking of the positive electrode active material can be prevented.

[0099] In step S14, a composite oxide containing lithium and a transition metal M that has been synthesized in advance can also be used. In this case, steps S11 to S13 can be omitted. By performing step S15 on a composite oxide that has been synthesized in advance, a composite oxide with a smooth surface can be obtained.

[0100] It is conceivable that the lithium in the composite oxide may be reduced by the initial heating. This reduction in lithium may make it easier for the additive elements, which will be described in the next step S20_1, to enter the composite oxide. Furthermore, if the additive elements are added to a composite oxide with a smooth surface, the additive elements can be added evenly, so it is preferable to add the additive elements after the initial heating. The step of adding the additive elements will be described using FIG. 2B.

[0101] <Step S20_1> and <Step S21_1> Details of step S20_1 shown in Fig. 2A are shown in Fig. 2B. In step S21_1 of Fig. 2B, an additive element A1 source (A1 source) to be added to the composite oxide is prepared. In order to compensate for the lithium lost by the initial heating, a lithium source may be prepared together with the additive element A1 source.

[0102] The additional element A1 can be one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic.

[0103] When magnesium is selected as the additional element A1, the source of the additional element A1 can be called a magnesium source (Mg source). As the magnesium source, magnesium fluoride, magnesium oxide, magnesium hydroxide, magnesium carbonate, or the like can be used. Furthermore, a plurality of the above-mentioned magnesium sources may be used.

[0104] When fluorine is selected as the additional element A1, the source of the additional element A1 can be called a fluorine source (F source). Examples of the fluorine source that can be used include lithium fluoride, magnesium fluoride, aluminum fluoride, titanium fluoride, cobalt fluoride, nickel fluoride, zirconium fluoride, vanadium fluoride, manganese fluoride, iron fluoride, chromium fluoride, niobium fluoride, zinc fluoride, calcium fluoride, sodium fluoride, potassium fluoride, barium fluoride, cerium fluoride, lanthanum fluoride, and sodium aluminum hexafluoride. Among these, lithium fluoride is preferred because it has a relatively low melting point of 848°C and is easily melted in the heating step described below. Note that FIG. 2B shows an example in which a Mg source and a F source are used as the source of the additional element A1.

[0105] Magnesium fluoride can be used as both a fluorine source and a magnesium source, and lithium fluoride can be used as a lithium source. Another lithium source that can be used in step S21_1 is lithium carbonate.

[0106] In this embodiment, lithium fluoride is prepared as the fluorine source, and magnesium fluoride is prepared as the fluorine source and magnesium source. Lithium fluoride and magnesium fluoride are prepared in the form of LiF:MgF 2 When the molar ratio of lithium fluoride and magnesium fluoride is about LiF:MgF = 65:35, the effect of lowering the melting point is maximized. On the other hand, if the amount of lithium fluoride is too large, there is a concern that the lithium will be excessive and the cycle characteristics will deteriorate. Therefore, in this embodiment, the molar ratio of lithium fluoride and magnesium fluoride is LiF:MgF 2 =x:1 (0≦x≦1.9), and LiF:MgF 2 =x:1 (0.1≦x≦0.5) is more preferable, and LiF:MgF 2 = x:1 (x = 0.33 or its vicinity) is more preferable. Note that "in the vicinity" refers to a value that is greater than 0.9 times and less than 1.1 times the value.

[0107] At the same time, the amount of magnesium added is 2 , typically LiCoO 2The content of magnesium relative to the number of Co atoms is preferably greater than 0.1 atomic % and less than 3 atomic %, more preferably greater than 0.5 atomic % and less than 2 atomic %, and even more preferably greater than 0.5 atomic % and less than 1 atomic %. If the amount of magnesium added is 0.1 atomic % or less, the initial discharge capacity is high, but repeated high-voltage charging can cause a rapid decrease in discharge capacity. If the amount of magnesium added exceeds 0.1 atomic %, that is, greater than 0.1 atomic % and less than 3 atomic %, both the initial discharge characteristics and charge-discharge cycle characteristics are good even after repeated high-voltage charging. On the other hand, if the amount of magnesium added exceeds 3 atomic %, the initial discharge capacity is low, and the charge-discharge cycle characteristics tend to gradually deteriorate.

[0108] 2B, the magnesium source and the fluorine source are mixed while being pulverized. This step can be performed under the pulverization conditions and the mixing conditions selected from those described in step S12.

[0109] If necessary, a heating step may be performed after step S22_1. In this case, the heating step can be performed under heating conditions selected from those described in step S13. The heating time is preferably 2 hours or more, and the heating temperature is preferably 800° C. or higher and 1100° C. or lower.

[0110] 2B, the pulverized and mixed material is recovered to obtain an additional element A1 source (A1 source). Note that the additional element A1 source shown in step S23_1 may contain multiple raw materials, such as an Mg source and an F source, and in this case, the A1 source may be called a mixture.

[0111] <Step S31> Next, in step S31 shown in FIG. 2A, the composite oxide and the additive element Al source (Al source) are mixed. The number of atoms A of the transition metal M in the composite oxide containing lithium and the transition metal M is M and the number of magnesium atoms A contained in the additive element A1. Mg The ratio of A M : A Mg = 100:y (0.1 ≦ y ≦ 6), and A M : A MgIt is more preferable that y=100:y (0.3≦y≦3).

[0112] The mixing in step S31 is preferably performed under milder conditions than the conditions for pulverization and mixing in step S12 so as not to destroy the composite oxide. For example, it is preferable to perform the mixing under conditions with a lower rotation speed or a shorter time than in step S12. Furthermore, a dry method is more preferable than a wet method because the conditions are milder.

[0113] The mixing is preferably carried out in an atmosphere having a dew point of −100° C. or higher and −10° C. or lower. For example, the mixing can be carried out in a dry room. The atmosphere in the dry room is dry air.

[0114] <Step S32> Next, in step S32 of Fig. 2A, the mixed materials are recovered to obtain a mixture 903. When recovering, the mixture 903 may be crushed to break up any agglomerated material. The mixture 903 may be sieved to further break up any agglomerated material. Sieving may be performed after crushing, or sieving may be performed while crushing, or sieving may be performed only instead of crushing.

[0115] In this embodiment, a method of adding lithium fluoride as a fluorine source and magnesium fluoride as a magnesium source to a composite oxide that has undergone initial heating has been described, but the present invention is not limited to the above method. In step S11, that is, in the stage of starting materials for the composite oxide, a magnesium source, a fluorine source, etc. can be prepared together with a Li source and an M source, and the process can proceed to step S12. Thereafter, in step S13, heating is performed to obtain LiMO with added magnesium and fluorine. 2 In this case, it is not necessary to separate the steps S11 to S14 from the steps S21_1 to S23_1. This method can be said to be simple and highly productive.

[0116] Alternatively, a composite oxide to which magnesium and fluorine have been added in advance may be used. If a composite oxide to which magnesium and fluorine have been added is used, the processes of steps S11 to S32 and step S20_1 can be omitted. This method can be said to be simple and highly productive.

[0117] Alternatively, a magnesium source and a fluorine source may be further added to a composite oxide to which magnesium and fluorine have been added in advance in step S20_1. Instead of or in addition to the magnesium source and the fluorine source, a nickel source and an aluminum source may be added.

[0118] 2A, the mixture 903 is heated. The heating conditions can be selected from those described in step S13. The heating time is preferably 2 hours or more.

[0119] Here, a supplementary note about the heating temperature will be given. The lower limit of the heating temperature in step S33 is 2 The temperature at which the reaction between the composite oxide and the additive element A1 source proceeds must be equal to or higher than the temperature at which the reaction between the composite oxide and the additive element A1 source proceeds. The temperature at which the reaction proceeds is the temperature at which the elements contained in the composite oxide and the additive element A1 source can diffuse into each other, and may be lower than the melting points of these materials. An oxide will be used as an example to explain this, but the Tammann temperature T d (Melting point T m It is known that solid-phase diffusion occurs at a temperature above which the heating temperature in step S33 is 500° C. or higher.

[0120] Of course, the reaction proceeds more easily when the temperature is equal to or higher than the temperature at which at least a part of the mixture 903 melts. 2 When LiF and MgF 2 Since the eutectic point of is around 742°C, the lower limit of the heating temperature in step S33 is preferably set to 742°C or higher.

[0121] Also, LiCoO 2 :LiF:MgF 2 A mixture 903 obtained by mixing the components so that the molar ratio was 100:0.33:1 exhibits an endothermic peak at around 830°C in differential scanning calorimetry (DSC). Therefore, the lower limit of the heating temperature is more preferably 830°C or higher.

[0122] A higher heating temperature is preferable because the reaction proceeds more easily, the heating time is shorter, and productivity is higher.

[0123] The upper limit of the heating temperature is set to be lower than the decomposition temperature of the composite oxide. For example, LiCoO 2 In this case, the temperature is set to be lower than the decomposition temperature of 1130°C. At temperatures close to the decomposition temperature, a small amount of LiMO 2 There is concern about the decomposition of LiMO. 2 When decomposition occurs, unnecessary reaction products are generated in the composite oxide, typically Co in the case of lithium cobalt oxide. 3 O 4 Therefore, the temperature is more preferably 1000°C or lower, even more preferably 950°C or lower, and even more preferably 920°C or lower.

[0124] In consideration of these, the heating temperature in step S33 is preferably 500°C or higher and lower than 1130°C, more preferably 500°C or higher and lower than 1000°C, even more preferably 500°C or higher and lower than 950°C, even more preferably 500°C or higher and lower than 920°C, and even more preferably 500°C or higher and lower than 900°C. Also, it is preferably 742°C or higher and lower than 1130°C, more preferably 742°C or higher and lower than 1000°C, even more preferably 742°C or higher and lower than 950°C, even more preferably 742°C or higher and lower than 920°C, and even more preferably 742°C or higher and lower than 900°C. Also, it is preferably 800°C or higher and lower than 1130°C, more preferably 800°C or higher and lower than 1000°C, even more preferably 800°C or higher and lower than 950°C, even more preferably 800°C or higher and lower than 920°C, and even more preferably 800°C or higher and lower than 900°C. Furthermore, the temperature is preferably 830°C or higher and lower than 1130°C, more preferably 830°C or higher and 1000°C or lower, even more preferably 830°C or higher and 950°C or lower, even more preferably 830°C or higher and 920°C or lower, and even more preferably 830°C or higher and 900°C or lower.

[0125] Furthermore, when heating the mixture 903, it is preferable to control the partial pressure of fluorine or fluoride originating from a fluorine source or the like in the processing chamber or the crucible within an appropriate range. In the manufacturing method described in this embodiment, some materials, for example, LiF, which is a fluorine source, may function as a flux. This function allows the heating temperature to be controlled within a range of 1000 saturation points.2 ) can be lowered to a temperature lower than the decomposition temperature, for example, 742°C or higher and 950°C or lower, and additive elements A1 such as magnesium can be distributed in the surface layer portion, thereby producing a positive electrode active material with good characteristics.

[0126] However, LiF may sublimate when heated, and since LiF has a lower specific gravity in gaseous state than oxygen, it is conceivable that the amount of LiF in the mixture 903 will decrease. This will weaken its function as a flux. Therefore, it is necessary to heat the mixture while suppressing the sublimation of LiF. Even if LiF is not used as a fluorine source, etc., LiMO 2 There is also a possibility that Li on the surface reacts with F in the fluorine source to produce LiF, which may then sublime. Therefore, even if a fluoride with a higher melting point than LiF is used, it is still necessary to suppress sublimation.

[0127] Therefore, it is preferable to heat the mixture 903 in an atmosphere containing LiF, that is, to heat the mixture 903 in a state where the partial pressure of LiF in the processing chamber is high. Such heating can suppress sublimation of LiF in the mixture 903. In addition, by placing a lid on the container as described above, it is also possible to suppress sublimation of LiF in the mixture 903.

[0128] The heating in this step is preferably performed so as not to stick together the mixture 903. If the mixture 903 sticks together during heating, the contact area with oxygen in the atmosphere decreases and the path along which the additional element A1 (e.g., magnesium and / or fluorine) diffuses is blocked, which may make it difficult for the additional element A1 (e.g., magnesium and / or fluorine) to diffuse.

[0129] Furthermore, it is believed that uniform distribution of the additive element A1 (e.g., fluorine) in the surface layer portion results in a smooth cathode active material with few irregularities. Therefore, in order to maintain or further smooth the surface after the heating in step S15 in this process, it is preferable that the mixture 903 does not stick to itself.

[0130] The heating time is determined by the heating temperature, the LiMO 2 It changes depending on the size and composition of LiMO.2 When the median diameter (D50) is small, a lower temperature or a shorter time may be more preferable than when the median diameter (D50) is large. The median diameter (D50) can be determined using a laser diffraction particle size distribution analyzer.

[0131] LiMO in step S14 of FIG. 2 When lithium cobalt oxide is used as the catalyst, and the median diameter (D50) of the lithium cobalt oxide is about 12 μm, such as 10 μm or more and 14 μm or less, the heating temperature in step S33 is preferably, for example, 800° C. or more and 920° C. or less, and more preferably 850° C. or more and 920° C. or less. The heating time in step S33 is, for example, more preferably 10 hours or more, and even more preferably 20 hours or more. When the median diameter (D50) is large, the composite oxide (LiMO 2 ) increases in volume, and therefore, internal stress is relaxed or removed in the bulk layer of the composite oxide, and therefore, a longer heating time may be required. If the median diameter (D50) is large, it takes time for the additive elements A1, including magnesium, to be uniformly distributed in the surface layer portion, and as described above, the heating time may be longer. The median diameter (D50) of lithium cobalt oxide may increase after heat treatment, but it is preferable that the median diameter (D50) be 10 μm or more and 14 μm or less even after heat treatment. In other words, it is preferable that the median diameter (D50) of the positive electrode active material be 10 μm or more and 14 μm or less.

[0132] LiMO in step S14 2When lithium cobalt oxide is used as the sintering agent, and the median diameter (D50) of the lithium cobalt oxide is about 7 μm, such as 5 μm or more and 9 μm or less, the heating temperature in step S33 is preferably in the same range as the heating temperature when the median diameter (D50) is about 12 μm. On the other hand, the heating time in step S33 can be shorter than the heating time when the median diameter (D50) is about 12 μm. For example, a heating time of 1 hour or more and 10 hours or less is preferable, and 5 hours or more and 10 hours or less is more preferable. When the median diameter (D50) is small, the time for the additional element A1, including magnesium, to be distributed in the surface layer portion is shortened, and therefore the heating time can be shortened as described above. When the median diameter (D50) is small, the composite oxide (LiMO 2 ) becomes smaller, the time required to temper or anneal the bulk layer of the composite oxide can be shortened. Although the median diameter (D50) of lithium cobalt oxide may increase after heat treatment, it is preferable that the median diameter (D50) remains 5 μm or more and 9 μm or less even after heat treatment. In other words, it is preferable that the median diameter (D50) of the positive electrode active material remains 5 μm or more and 9 μm or less.

[0133] After step S33, a step of further adding an additional element different from the additional element A1 may be provided. This step will be described with reference to FIG. 2C.

[0134] <Step S20_2> and <Step S21_2> Details of step S20_2 shown in Fig. 2A are shown in Fig. 2C. In step S21_2 of Fig. 2C, an additive element A2 source (A2 source) to be added to the composite oxide is prepared. A lithium source may be prepared together with the additive element A2 source.

[0135] The additive element A2 can be one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic. It is preferable that the additive element A2 be at least an element not selected as the additive element A1, but it may also contain an element selected as the additive element A1. Note that FIG. 2C shows an example in which a Ni source and an Al source are used as sources of the additive element A2.

[0136] In this embodiment, nickel hydroxide is prepared as the nickel source, and aluminum hydroxide is prepared as the aluminum source. Nickel oxide or nickel carbonate can be used instead of nickel hydroxide. Aluminum oxide or aluminum carbonate can be used instead of aluminum hydroxide.

[0137] <Step S22_2> Next, in step S22_2 shown in Fig. 2C, the nickel source is mixed while being pulverized, and further the aluminum source is mixed while being pulverized. This step can be performed under the pulverization conditions and mixing conditions selected from those described in step S12. Note that this step can also be performed by combining the nickel source and the aluminum source and then mixing them while being pulverized, as in step S22_1 in Fig. 2B.

[0138] If necessary, a heating step can be performed after step S22_2. In this case, the heating step can be performed under the heating conditions selected from those described in step S13.

[0139] <Step S23_2> Next, in step S23_2 shown in FIG. 2C, the material crushed or mixed as described above is recovered to obtain a source of the additional element A2 (A2 source).

[0140] <Step S34> Next, in step S34 shown in FIG. 2A, the composite oxide that has been heated in step S33 is mixed with the additive element A2 source (A2 source). As described above, a plurality of additive element A2 sources (A2 sources) can be prepared. The number of atoms A of the transition metal M in the composite oxide is M and the number of nickel atoms A contained in the additive element A2.Ni The ratio of A M : A Ni = 100:y (0.1 ≤ y ≤ 3), and A M : A Ni It is more preferable that the number of atoms of the transition metal M in the composite oxide is 100:y (0.3≦y≦1). M and the number of aluminum atoms A contained in the additive element A2. Al The ratio of A M : A Al = 100:y (0.1 ≤ y ≤ 3), and A M : A Al It is more preferable that y=100:y (0.3≦y≦1).

[0141] The mixing conditions in step S34 can be selected from the mixing conditions described in step S31.

[0142] <Step S35> Next, in step S35 of Fig. 2A, the mixed materials are recovered to obtain a mixture 904. When recovering, the mixture 904 can be crushed to break up any agglomerations. The mixture 904 can also be sieved to further break up any agglomerations. Sieving can be performed after crushing, sieving can be performed while crushing, or sieving can be performed alone instead of crushing.

[0143] 2A, the mixture 904 is heated. The heating conditions can be selected from those described in step S33. The heating time is preferably 2 hours or more.

[0144] The heating temperature in step S36, as in step S33, is preferably 500°C to 1130°C, more preferably 500°C to 1000°C, even more preferably 500°C to 950°C, and even more preferably 500°C to 900°C. Also, it is preferably 742°C to 1130°C, more preferably 742°C to 1000°C, even more preferably 742°C to 950°C, and even more preferably 742°C to 900°C. Also, it is preferably 800°C to 1100°C, or 830°C to 1130°C, more preferably 830°C to 1000°C, more preferably 830°C to 950°C, and even more preferably 830°C to 900°C.

[0145] The heating in this step is preferably performed so as not to stick together the mixture 904. If the mixture 904 sticks together during heating, the contact area with oxygen in the atmosphere will decrease and the path along which the additional element A2 diffuses will be blocked, which may result in a poor distribution of the additional element A2.

[0146] <Step S37> Next, in step S37 shown in FIG. 2A , the heated material is recovered and crushed as necessary to obtain the positive electrode active material 10. At this time, it is preferable to further sieve the recovered positive electrode active material 10. Through the above steps, the positive electrode active material 10 of one embodiment of the present invention can be produced. The positive electrode active material of one embodiment of the present invention has a smooth surface. The above is an example of a method for producing a positive electrode active material.

[0147] [Positive Electrode Active Material] A cross section of a positive electrode active material 10 obtainable by the above-described manufacturing method will be described using FIG. 3A. Also, unlike FIG. 3A, FIG. 3B shows a cross section of the positive electrode active material 10, with the grain boundaries 11 clearly indicated by dashed lines. Both the positive electrode active material 10 shown in FIGS. 3A and 3B have a surface layer portion 10a and an interior portion (the interior portion will be referred to as the "bulk portion") 10b, with the boundary between them indicated by a dashed line. It is more preferable that the surface layer portion 10a covers 90% or more of the bulk portion 10b. The dashed lines in FIGS. 3A and 3B are examples, and the dashed line in FIG. 3B is also an example, and the proportion of the surface layer portion covered is also an example.

[0148] The surface layer portion 10a does not have to cover the entire bulk portion 10b. Figures 3A and 3B show a cathode active material 10 in which the surface layer portion 10a covers 50% or more, specifically 65% ​​to 75%, of the outer periphery of the bulk portion 10b. For example, as shown in Figure 3B, the cathode active material 10 may have a region in which the bulk portion 10b is exposed.

[0149] The crystal grain boundary 11 shown in FIG. 3B refers to, for example, a portion where the positive electrode active material 10 is adhered to itself, a portion where the crystal orientation changes within the positive electrode active material 10, i.e., a portion where the repetition of bright and dark lines in an STEM image or the like becomes discontinuous, a portion containing many crystal defects, or a portion where the crystal structure is disordered. Crystal defects refer to defects that can be observed in a cross-sectional TEM (transmission electron microscope) image, a cross-sectional STEM image, or the like, and such defects can also be called a structure in which other elements have entered between lattices, or a cavity, etc. In other words, the crystal grain boundary 11 can be said to be one of the planar defects. The vicinity of the crystal grain boundary 11 refers to a region within 20 nm, preferably within 10 nm, of the center of the crystal grain boundary 11, and the vicinity of the grain boundary exists both inside and outside the particle. These can be distinguished by indicating the vicinity of the grain boundary inside the particle or the vicinity of the grain boundary outside the particle.

[0150] Because the positive electrode active material 10 contains a composite oxide containing a transition metal and oxygen capable of lithium insertion / extraction, the interface between a region containing a transition metal M (e.g., Co, Ni, Mn, Fe, etc.) that is oxidized and reduced upon lithium insertion / extraction and a region containing no transition metal M can be considered the "surface" of the positive electrode active material. The region containing no transition metal M may contain an additive element. Surfaces newly formed by slippage, cracks, and / or fractures may also be considered the surface of the positive electrode active material.

[0151] Again, in this specification, the surface layer portion 10a refers to, for example, a region within 50 nm, more preferably within 35 nm, even more preferably within 20 nm, and most preferably within 10 nm from the surface toward the interior. Alternatively, the surface layer portion may be referred to as the near-surface, near-surface region, or shell. The region within 50 nm, more preferably within 35 nm, even more preferably within 20 nm, and most preferably within 10 nm from the surface toward the interior refers to the depth direction along a perpendicular or approximately perpendicular direction from the surface. Perpendicular or approximately perpendicular to the surface refers to a direction that forms an angle of 80° or more and 100° or less with a tangent to the surface. Furthermore, the bulk portion 10b refers to a region deeper than the surface layer portion 10a. The bulk portion 10b may be referred to as the interior, or may be referred to as the core. The bulk portion 10b may include the central portion of the positive electrode active material.

[0152] The region of the positive electrode active material 10 where lithium is inserted and removed may be referred to as the "surface." Therefore, the "surface" can be considered to be a region of the positive electrode active material 10 that comes into contact with the electrolyte. For example, the surface of the positive electrode active material 10 includes the surface of the surface layer portion 10a, and in a region where the bulk portion 10b is exposed, the bulk portion 10b may be the surface.

[0153] Carbonate groups, hydroxyl groups, and the like that are chemically adsorbed after preparation of the positive electrode active material 10 are considered to be regions where lithium cannot be inserted or removed, and these do not constitute the surface of the positive electrode active material 10. Similarly, the electrolyte, binder, conductive material, or compounds derived from these that are attached to the positive electrode active material 10 do not constitute the surface of the positive electrode active material 10 either.

[0154] Furthermore, the "surface" of the positive electrode active material 10 in a cross-sectional STEM (scanning transmission electron microscope) image or the like refers to the boundary between an area where an electron beam combined image is observed and an area where it is not observed, and can be the outermost area where bright spots originating from the atomic nuclei of metal elements with atomic numbers larger than that of lithium are observed. The surface in a cross-sectional STEM image or the like can also be determined in conjunction with the results of an analysis with higher spatial resolution, such as electron energy loss spectroscopy (EELS).

[0155] The positive electrode active material must contain a transition metal capable of oxidation and reduction in order to maintain charge neutrality even when lithium ions are inserted and removed. The positive electrode active material 10 of one embodiment of the present invention primarily uses cobalt as the transition metal M responsible for the oxidation and reduction reaction. However, in addition to cobalt, at least one or more selected from nickel and manganese may also be used. It is preferable for the positive electrode active material 10 to contain 75 atomic % or more, preferably 90 atomic % or more, and more preferably 95 atomic % or more of cobalt among the transition metals M contained therein, as this has many advantages, such as relatively easy synthesis, ease of handling, and excellent cycle characteristics.

[0156] When nickel is used as the transition metal M in the positive electrode active material 10 at 33 atomic % or more, preferably at 60 atomic % or more, and more preferably at 80 atomic % or more, the raw material may be cheaper than when cobalt is used in large amounts, and the discharge capacity per weight may increase, which is preferable.

[0157] The additive element A (additive element A1 and additive element A2) contained in the positive electrode active material 10 will be listed again. It is preferable to use one or more elements selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic.

[0158] That is, the positive electrode active material 10 can be called lithium cobalt oxide to which the additive element A has been added. As will be described later, the additive element A can further stabilize the crystal structure of the positive electrode active material 10.

[0159] The additional element A does not necessarily have to contain one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic.

[0160] For example, if positive electrode active material 10 is substantially free of manganese as additive element A, the advantages of relatively easy synthesis and handling, and excellent cycle characteristics, are further enhanced. The weight of manganese contained in positive electrode active material 10 is preferably, for example, 600 ppm or less, more preferably 100 ppm or less. The weight of manganese can be analyzed using, for example, a glow discharge mass spectrometer (GD-MS).

[0161] <Crystal Structure> Using Figs. 4 to 8, LixCoO 2 The change in crystal structure accompanying the change in x in the positive electrode active material 10 usable as one embodiment of the present invention will be described by comparing it with a conventional positive electrode active material. The crystal structure of the positive electrode active material 10 usable as one embodiment of the present invention is shown in FIG. 4, and the crystal structure of the conventional positive electrode active material is shown in FIG. 5. The conventional positive electrode active material shown in FIG. 5 is a lithium cobalt oxide (LiCoO 2 In this specification, "not containing any particular added elements" refers to a case where the amount of added elements is below the lower limit of detection when measured using analytical means, or, if the amount is at the very edge of the lower limit of detection, to a level that does not affect the presence or absence of an action or effect.

[0162] <Li x CoO 2 When x is 1, the positive electrode active material 10 usable as one embodiment of the present invention is Li x CoO 2 In the case where x=1, that is, in the discharged state, it is preferable that the material has a layered rock-salt type crystal structure belonging to the space group R-3m. In this crystal structure, lithium occupies octahedral sites and CoO 2 There are three layers. Therefore, this crystal structure is sometimes called an O3 type crystal structure. 2 The layer refers to a structure in which an octahedral structure in which cobalt is six-coordinated with oxygen is continuous on a plane in an edge-sharing state. 2 The layer is sometimes referred to as a layer consisting of cobalt and oxygen octahedra. x CoO 2The crystal structure when x is 1 is designated as R-3m(O3). x CoO 2 When x is 1 in the formula, the crystal structure is the same as the crystal structure shown in FIG. 4, and is similarly denoted by R-3m(O3).

[0163] The layered rock-salt composite oxide has a high discharge capacity, two-dimensional lithium ion diffusion paths, and is suitable for lithium ion insertion / extraction reactions, making it an excellent positive electrode active material for lithium ion batteries. Therefore, it is preferable that the bulk portion 10b, which accounts for the majority of the positive electrode active material 10, has a layered rock-salt crystal structure.

[0164] The crystal structure of the surface layer 10a of the cathode active material 10 usable as one embodiment of the present invention does not have to be a layered rock salt type. The surface layer 10a preferably has a function of reinforcing the bulk portion 10b, which is made up of octahedra of cobalt and oxygen, so that the layered structure of the bulk portion 10b is not destroyed even when lithium is removed from the cathode active material 10 upon charging. Alternatively, the surface layer 10a preferably functions as a barrier film for the cathode active material 10. Alternatively, the surface layer 10a, which is the outer periphery of the cathode active material 10, preferably reinforces the cathode active material 10. Here, "reinforcement" refers to suppressing structural changes in the surface layer 10a and bulk portion 10b of the cathode active material 10, such as oxygen desorption, and / or suppressing oxidative decomposition of the electrolyte on the surface of the cathode active material 10.

[0165] The surface layer 10a is the region from which lithium ions are first released during charging, and is a region where the lithium concentration is likely to be lower than that of the bulk portion 10b. In addition, when lithium ions are released, some of the bonds of the atoms on the surface of the positive electrode active material 10 in the surface layer 10a are broken. Therefore, the surface layer 10a is likely to become unstable, and is a region where the crystal structure is likely to change, that is, where deterioration is likely to begin. On the other hand, if the surface layer 10a can be made sufficiently stable, Li x CoO 2 When x is small, for example, even if x is 0.24 or less, CoO 2 Furthermore, the CoO 2 The misalignment of the layers can be suppressed.

[0166] In order to give the surface layer portion 10a a stable composition and crystal structure, the surface layer portion 10a preferably contains an additive element A, and more preferably contains a plurality of additive elements A. Furthermore, the surface layer portion 10a preferably has a higher concentration of one or more selected from the additive elements A than the bulk portion 10b. Furthermore, it is preferable that the one or more selected from the additive elements A contained in the positive electrode active material 10 have a concentration gradient. Furthermore, it is more preferable that the distribution of the additive element A in the positive electrode active material 10 differs depending on the additive element A. For example, it is more preferable that the depth from the surface of the concentration peak differs depending on the additive element A. The concentration peak here refers to the maximum concentration value in the surface layer portion 10a or within 50 nm from the surface.

[0167] Here, the above concentration gradient and concentration peak will be explained with reference to the conceptual diagrams of FIGS. 3C to 3F.

[0168] 3C and 3D show enlarged views of the vicinity of A-B in FIG. 3A. 3C and 3D are cross-sectional views of the surface layer having the (001) plane (hereinafter referred to as the (001) plane, and may also be referred to as the c-plane or basal plane), that is, cross-sectional views of the region oriented in (001). In the layered rock salt type crystal structure, cations are arranged parallel to the (001) plane. This is due to the CoO 2 It can be said that the structure is one in which the CoO layer and the lithium layer are alternately stacked parallel to the (001) plane. Therefore, the diffusion path of lithium ions exists parallel to the (001) plane. 2 The layer is relatively stable, so CoO 2 The (001) plane on which the layer is present is relatively stable, and the main diffusion path of lithium ions during charge and discharge is not exposed on the (001) plane.

[0169] FIG. 3C shows the distribution of magnesium as an example of the added element A. The shading in FIG. 3C corresponds to the change in magnesium concentration. The (001) plane is CoO 2Since the layer is relatively stable, the additional element A may not be detected. When the additional element A is detected, FIG. 3C shows an example of the distribution of the additional element A, in which the additional element A is present at the highest concentration at or near the surface of the surface layer portion 10a, and the concentration of the additional element A decreases toward the bulk portion 10b. It can be said that there is a concentration peak of magnesium or the like at the position showing the highest concentration. The decrease in concentration may also be referred to as a concentration gradient. In this specification, the additional element A that shows a distribution as shown in FIG. 3C on the (001) plane will be referred to as the additional element X.

[0170] FIG. 3D shows the distribution of aluminum as another example of the added element A. The shading in FIG. 3D corresponds to the change in aluminum concentration. The (001) plane is CoO 2 Because the layer is relatively stable, the additional element A may not be detected. When the additional element A is detected, FIG. 3D shows an example of the distribution of the additional element A, in which the additional element A is present at the highest concentration at a position deeper than the surface or near the surface in the surface layer portion 10a, and the concentration of the additional element A decreases toward the surface and bulk portion 10b. It can be said that there is an aluminum concentration peak at the position showing the highest concentration, and the aluminum concentration peak position may be located slightly deeper than the concentration peak positions of the magnesium and other elements. The decrease in concentration may also be referred to as a concentration gradient. In this specification, the additional element A that exhibits a distribution as shown in FIG. 3D on the (001) plane will be referred to as the additional element Y.

[0171] Depending on the element of the additional element A, a distribution like that of the additional element X or a distribution like that of the additional element Y may be exhibited, and the distributions may differ from each other. Furthermore, depending on the element of the additional element A, a concentration peak position like that of the additional element X or a concentration peak position like that of the additional element Y may be exhibited, and the concentration peak positions may differ from each other.

[0172] Figures 3E and 3F are enlarged views of the vicinity of C-D in Figure 3A. Figures 3E and 3F can be said to be cross-sectional views of a surface layer having a plane other than the (001) plane (hereinafter, sometimes referred to as an ab plane or an edge plane), and in a layered rock-salt crystal structure, a plane other than the (001) plane is a plane where a diffusion path for lithium ions exists.

[0173] In FIG. 3E , which shows a plane other than the (001) plane, the distribution of magnesium or the like is shown as an example of the additional element X. Compared to the (001) plane in FIG. 3C , the concentration of the additional element X may be higher in the plane other than the (001) plane in FIG. 3E . The concentration peak of magnesium or the like may be located on or near the surface of the surface layer 10 a, and may exhibit a higher intensity than the concentration peak in the (001) plane in FIG. 3C . Furthermore, the additional element X may be distributed over a wide range in the plane other than the (001) plane in FIG. 3E .

[0174] 3F shows the distribution of aluminum and the like as an example of the added element Y. The aluminum concentration peak is preferably located in a region of 5 nm to 50 nm from the surface toward the inside, whether on the (001) plane in FIG. 3D or on a plane other than the (001) plane in FIG. 3F. Depending on the heat treatment conditions, the aluminum concentration peak may be deeper on a plane other than the (001) plane in FIG. 3F than on the (001) plane in FIG. 3D.

[0175] In this way, the distribution of the additive element may differ depending on the surface direction of the positive electrode active material.

[0176] Again, the diffusion paths of lithium ions exist on surfaces other than the (001) plane, and the diffusion paths of lithium ions are exposed on surfaces other than the (001) plane. Therefore, as shown in Figures 3E and 3F, the surface layer portion 10a corresponding to the surfaces other than the (001) plane is an important region for maintaining the diffusion paths of lithium ions, and at the same time, it is the region from which lithium ions are first desorbed and therefore prone to instability. Therefore, in order to maintain the crystal structure of the entire positive electrode active material 10, it is preferable to preferentially reinforce the surfaces other than the (001) plane and the corresponding surface layer portion 10a. In other words, it is preferable that the additive element A is preferentially present on the surfaces other than the (001) plane and the corresponding surface layer portion 10a.

[0177] As described in the above manufacturing method, LiCoO formed through initial heating 2 In the case of a manufacturing method in which the additive element is mixed and heated, the additive element spreads through the diffusion path of lithium ions, and therefore, it is easy to make the distribution of the additive element in the planes other than the (001) plane and the surface layer portion 10a corresponding to those planes fall within a preferred range, as shown in FIGS.

[0178] Although it has been stated that the surface of the positive electrode active material 10 is preferably smooth and has few irregularities, the entire positive electrode active material 10 does not necessarily have to be smooth. For example, the positive electrode active material 10 may have irregularities due to slips occurring on a surface parallel to the (001) plane, for example, on a surface where lithium is arranged. Slips are also called stacking faults. For example, pressing is performed when preparing the positive electrode, and the pressing causes LiCoO 2 The deformation can occur along the lattice fringe direction (the ab plane direction), and this deformation is also included in slip. Deformation can include the lattice fringes shifting back and forth. When the lattice fringes shift back and forth, a step occurs on the surface in the direction perpendicular to the lattice fringes (the c-axis direction).

[0179] Furthermore, the surface resulting from the slip and its surface layer 10a are often the (001) plane, and the surface layer 10a corresponding to the (001) plane may not contain any added elements or may contain elements below the detection limit. As mentioned above, the (001) plane does not expose the diffusion path of lithium ions and is relatively stable, so there is almost no problem even if the added elements are not present or are below the detection limit.

[0180] The composition is LiCoO 2 In the composite oxide having a layered rock salt type crystal structure of R-3m, cobalt is arranged parallel to the (001) plane. 2 Among the atoms, cobalt, which has the largest atomic number, has the highest brightness. Therefore, in a HAADF-STEM image, the arrangement of bright atoms can be considered to be the arrangement of cobalt. The repetition of this arrangement of bright atoms is synonymous with crystal fringes or lattice fringes.

[0181] Next, the additive elements will be described. Magnesium, which is one of the additive elements X, is divalent, and magnesium ions are more stable at the lithium site than at the cobalt site in the layered rock-salt crystal structure, so they are more likely to enter the lithium site. The presence of magnesium at an appropriate concentration at the lithium site in the surface layer portion 10a makes it easier to reinforce the layered rock-salt crystal structure of the bulk portion 10b, etc. This is because magnesium present at the lithium site is easily absorbed by CoO 2 It is presumed that this is because it functions as a pillar supporting the layers. x CoO 2 When x in the formula (1) is, for example, 0.24 or less, the desorption of oxygen around the magnesium can be suppressed. Furthermore, the presence of magnesium is expected to increase the density of the positive electrode active material 10. Furthermore, a high magnesium concentration in the surface layer portion 10a is expected to improve corrosion resistance to hydrofluoric acid produced by decomposition of the organic solvent.

[0182] At an appropriate concentration, magnesium does not adversely affect the intercalation and deintercalation of lithium during charging and discharging, providing the above benefits. However, excessive magnesium may adversely affect the intercalation and deintercalation of lithium. Furthermore, its effect on stabilizing the crystal structure may be reduced. This is thought to be due to magnesium occupying cobalt sites in addition to lithium sites. In addition, unnecessary magnesium compounds (oxides, fluorides, etc.) that do not substitute for either the lithium or cobalt sites may segregate on the surface of the positive electrode active material and become resistance components in lithium-ion batteries. Furthermore, as the magnesium concentration in the positive electrode active material increases, the discharge capacity of the positive electrode active material may decrease. This is thought to be due to excessive magnesium occupancy at the lithium sites, reducing the amount of lithium contributing to charging and discharging.

[0183] Therefore, it is preferable that the amount of magnesium contained in the entire positive electrode active material 10 is appropriate. For example, the number of magnesium atoms is preferably 0.001 to 0.1 times the number of cobalt atoms, more preferably more than 0.01 to less than 0.04 times, and even more preferably about 0.02 times. The amount of magnesium contained in the entire positive electrode active material 10 here may be a value obtained by performing elemental analysis of the entire positive electrode active material 10 using, for example, glow discharge mass spectrometry (GD-MS) or inductively coupled plasma mass spectrometry (ICP-MS), or may be based on the value of the composition of raw materials in the process of producing the positive electrode active material 10.

[0184] Nickel, which is one of the additional elements X, can exist on either the cobalt site or the lithium site. When nickel exists on the cobalt site, its oxidation-reduction potential is lower than that of cobalt, which is preferable as it leads to an increase in discharge capacity.

[0185] Furthermore, when nickel is present at the lithium site, the layer structure consisting of octahedra of cobalt and oxygen can be prevented from shifting. Also, the volume change caused by charge and discharge is prevented. Also, the elastic modulus increases, that is, the material becomes hard. This is because nickel present at the lithium site and CoO 2 It is thought that this is because they function as pillars supporting the layers.

[0186] On the other hand, an excess of nickel is undesirable because it increases the influence of strain due to the Jahn-Teller effect, and may also adversely affect the insertion and extraction of lithium.

[0187] Therefore, it is preferable that the amount of nickel contained in the entire positive electrode active material 10 is appropriate. For example, the number of nickel atoms contained in the positive electrode active material 10 is preferably greater than 0% and less than 7.5% of the number of cobalt atoms, preferably 0.05% to 4%, preferably 0.1% to 2%, and more preferably 0.2% to 1%. Alternatively, it is preferably greater than 0% and less than 4%. Alternatively, it is preferably greater than 0% and less than 2%. Alternatively, it is preferably 0.05% to less than 7.5%. Alternatively, it is preferably 0.05% to 2%. Alternatively, it is preferably 0.1% to less than 7.5%. Alternatively, it is preferably 0.1% to 4%. The amount of nickel shown here may be a value obtained by performing elemental analysis of the entire positive electrode active material using, for example, GD-MS, ICP-MS, or the like, or may be based on the value of the composition of raw materials in the process of producing the positive electrode active material.

[0188] Furthermore, aluminum, one of the additive elements Y, can exist at the cobalt site in the layered rock salt crystal structure. Because aluminum is a trivalent typical element and its valence does not change, lithium around the aluminum is less likely to move during charging and discharging. Therefore, the aluminum and its surrounding lithium function as pillars, suppressing changes in the crystal structure. Furthermore, aluminum has the effect of suppressing the elution of surrounding cobalt and improving continuous charging durability. Furthermore, because the Al—O bond is stronger than the Co—O bond, it can suppress the desorption of oxygen around the aluminum. These effects improve thermal stability. Therefore, a positive electrode active material containing aluminum as an additive element can improve safety when used in a lithium-ion battery. Furthermore, a positive electrode active material 10 can be obtained whose crystal structure is less likely to collapse even after repeated charging and discharging.

[0189] Furthermore, it is preferable that aluminum, which is one of the additional elements Y, is present at a position slightly deeper than the surface (specifically, that the aluminum concentration peak is in a region deeper than the concentration peak of the additional element X). Alternatively, it is preferable that the presence of aluminum, which is one of the additional elements Y, is confirmed in a region deeper than the deepest position where the presence of the additional element X is confirmed. This is because, if aluminum were to be substituted for a lithium site on the surface, lithium present in the vicinity of the aluminum substituted for the lithium site would be fixed, and this could hinder the diffusion path of lithium.

[0190] On the other hand, excessive aluminum may adversely affect lithium insertion and desorption. Therefore, it is preferable that the amount of aluminum contained in the entire positive electrode active material 10 is appropriate. For example, the number of aluminum atoms contained in the entire positive electrode active material 10 is preferably 0.05% to 4% of the number of cobalt atoms, preferably 0.1% to 2%, and more preferably 0.3% to 1.5%. Alternatively, 0.05% to 2% is preferable. Alternatively, 0.1% to 4% is preferable. The amount contained in the entire positive electrode active material 10 here may be, for example, a value obtained by performing elemental analysis of the entire positive electrode active material 10 using GD-MS, ICP-MS, or the like, or may be based on the value of the composition of raw materials in the process of producing the positive electrode active material 10.

[0191] Furthermore, fluorine, one of the additive elements X, is a monovalent anion. When a portion of the oxygen in the surface layer portion 10a is substituted with fluorine, the lithium desorption energy decreases. This is because the valence of the cobalt ion changes with lithium desorption (from trivalent to tetravalent in the absence of fluorine, and from divalent to trivalent in the presence of fluorine), resulting in different oxidation-reduction potentials. Therefore, when a portion of the oxygen in the surface layer portion 10a of the positive electrode active material 10 is substituted with fluorine, it can be said that desorption and insertion of lithium ions near the fluorine occurs more smoothly. Therefore, when used in a lithium ion battery, charge / discharge characteristics, large current characteristics, etc. can be improved. Furthermore, the presence of fluorine in the surface layer portion 10a, which has a surface that contacts the electrolyte, can effectively improve corrosion resistance against hydrofluoric acid. Furthermore, as will be described in a later embodiment, when the melting point of a fluoride, such as lithium fluoride, is lower than the melting point of another additive element source, it can function as a flux (also called a fluxing agent) that lowers the melting point of the other additive element source.

[0192] Furthermore, when the surface layer 10a contains both magnesium and nickel, there is a possibility that divalent magnesium can exist more stably near divalent nickel. x CoO 2 Even when the value of x in the formula is small, the elution of magnesium can be suppressed, which can contribute to the stabilization of the surface layer 10a.

[0193] Furthermore, having additive elements with different distributions, such as additive element X and additive element Y, in combination is preferable because it can stabilize the crystal structure in a wider region. For example, when the positive electrode active material 10 has both magnesium and nickel as the additive element X and aluminum as the additive element Y, it can stabilize the crystal structure in a wider region than when it has only one of the additive element X and the additive element Y. In this way, when the positive electrode active material 10 has both additive element X and additive element Y, the additive element Y, such as aluminum, is not essential to the surface because the surface stabilization can be sufficiently achieved by the additive element X, such as magnesium. Rather, it is preferable for aluminum to be widely distributed in a deep region, for example, a region with a depth from the surface of 5 nm to 50 nm, because this can stabilize the crystal structure in a wider region.

[0194] When a plurality of additive elements are contained as described above, the effects of the respective additive elements are synergistic and can contribute to further stabilization of the surface layer portion 10 a. In particular, when magnesium, nickel, and aluminum are contained, the effect of providing a stable composition and crystal structure is high and is therefore preferable.

[0195] However, if the surface layer 10a is occupied only by a compound of the additive element and oxygen, it is not preferable because it makes it difficult to insert and extract lithium. For example, it is not preferable for the surface layer 10a to be occupied only by MgO, a structure in which MgO and NiO(II) are solid-solved, and / or a structure in which MgO and CoO(II) are solid-solved. Therefore, it is preferable that the surface layer 10a contains at least cobalt and also contains lithium in a discharged state, so that a path for insertion and extraction of lithium is secured.

[0196] In order to ensure sufficient paths for lithium insertion and desorption, the surface layer 10a preferably has a higher cobalt concentration than magnesium. The surface layer 10a preferably has a higher cobalt concentration than nickel. The surface layer 10a preferably has a higher cobalt concentration than aluminum. The surface layer 10a preferably has a higher cobalt concentration than fluorine.

[0197] Furthermore, since there is a risk that an excessive amount of nickel may hinder the diffusion of lithium, it is preferable that the concentration of magnesium in the surface layer portion 10a is higher than that of nickel.

[0198] Furthermore, it is preferable that some of the additive elements, particularly magnesium and nickel, be present at a higher concentration in the surface layer portion 10a than in the bulk portion 10b, and that they also be present randomly and in a sparse manner in the bulk portion 10b. It is also preferable that aluminum, which is one of the additive elements, is also present randomly and in a sparse manner in the bulk portion 10b. When magnesium and aluminum are present at appropriate concentrations at the lithium sites in the bulk portion 10b, it has the effect of making it easier to maintain the layered rock-salt crystal structure, as described above. Furthermore, when nickel is present at an appropriate concentration in the bulk portion 10b, it can suppress the shift in the layered structure consisting of cobalt and oxygen octahedra, as described above. Furthermore, when magnesium and nickel are present together, a synergistic effect of suppressing magnesium elution can be expected, as described above.

[0199] Furthermore, due to the concentration gradient of the added element, it is preferable that the crystal structure of the lithium cobalt oxide continuously changes from the bulk portion 10b toward the surface portion 10a. In this case, it is preferable that the surface portion 10a has a composition and crystal structure that are more stable at room temperature (25°C) than the bulk portion 10b. For example, it is preferable that at least a portion of the surface portion 10a of the positive electrode active material 10 usable as one embodiment of the present invention has a rock salt type crystal structure. Alternatively, it is preferable that the surface portion 10a has both a layered rock salt type crystal structure and a rock salt type crystal structure. Alternatively, it is preferable that the surface portion 10a has characteristics of both a layered rock salt type crystal structure and a rock salt type crystal structure.

[0200] Furthermore, due to the concentration gradient of the added element, it is preferable that the crystal orientation of the surface layer portion 10a and the bulk portion 10b is approximately the same, or that the surface layer portion 10a and the bulk portion 10b are topotaxy.

[0201] In this specification, topotaxis refers to a three-dimensional structural similarity in which the crystal orientations roughly coincide, or to a crystallographically identical orientation, while epitaxy refers to a two-dimensional interface structural similarity.

[0202] The topotactic relationship between the surface layer portion 10 a and the bulk portion 10 b can reduce distortion of the crystal structure and / or misalignment of the atoms, thereby suppressing the cause of pits. In this specification, pits refer to holes formed by the progression of defects in the positive electrode active material.

[0203] <Li x CoO 2 When x is small in the positive electrode active material 10 usable as one embodiment of the present invention, due to the distribution of the additive element and / or the crystal structure as described above, x CoO 2 The crystal structure when x is small differs from that of conventional positive electrode active materials. Again, in this specification, "small x" means 0.1<x≦0.24.

[0204] First, conventional Li x CoO2 In the case of lithium cobalt oxide where x=0.5, which corresponds to a slightly small value of x, the symmetry of lithium is increased as shown in FIG. 5, and the lithium cobalt oxide has a crystal structure belonging to the monoclinic space group P2 / m. This structure has CoO in the unit cell. 2 There is one layer. Therefore, it is sometimes called monoclinic O1 type or O1 type. In Figure 5, the crystal structure with x = 0.5 is labeled P2 / m (monoclinic O1).

[0205] In addition, conventional Li x CoO 2 In the above formula, when x=0, lithium cobalt oxide has a crystal structure of the trigonal space group P-3m1 as shown in FIG. 5, and CoO 2 There is one layer. Therefore, this crystal structure is sometimes called trigonal O1 type or O1 type. In addition, the trigonal crystal is sometimes converted into a composite hexagonal lattice and called hexagonal O1 type. In Figure 5, the crystal structure with x = 0 is labeled P-3m1 (trigonal O1).

[0206] In addition, conventional Li x CoO 2 In the above formula, when x is small (x=0.12), lithium cobalt oxide has a crystal structure of the space group R-3m as shown in FIG. 5. This structure is similar to CoO, such as trigonal O1 type. 2 and LiCoO such as R-3m(O3). 2 It can also be said that this crystal structure is a structure in which the structure of and the structure of are stacked alternately. Therefore, this crystal structure is sometimes called an H1-3 crystal structure. In reality, the number of cobalt atoms per unit cell in the H1-3 crystal structure is twice that of other structures. However, in Figure 5 and other figures in this specification, to facilitate comparison with other crystal structures, the c-axis of the H1-3 crystal structure is shown as half the unit cell. In Figure 5, the crystal structure with x = 0.12 is labeled R-3m1 (H1-3).

[0207] In the H1-3 type crystal structure, the coordinates of cobalt and oxygen in the unit cell can be expressed as Co (0, 0, 0.42150 ± 0.00016), O1 (0, 0, 0.27671 ± 0.00045), and O2 (0, 0, 0.11535 ± 0.00045). O1 and O2 are each oxygen atoms. Which unit cell should be used to represent a certain crystal structure can be determined, for example, by Rietveld analysis using X-ray diffraction (abbreviated as XRD). In Rietveld analysis, the unit cell with the smallest GOF (goodness of fit) value is adopted.

[0208] When x is small, the corresponding Li x CoO 2 When charging and discharging are repeated so that x in the formula is 0.12 or less, conventional lithium cobalt oxide undergoes repeated changes in crystal structure (i.e., non-equilibrium phase changes) between the H1-3 type crystal structure and the R-3m(O3) structure in the discharged state, as shown in Figure 5.

[0209] However, these two crystal structures are different from CoO 2 As shown in the crystal structure labeled R-3m1 (H1-3) in FIG. 5, in the H1-3 type crystal structure, CoO 2 The layer is significantly different from the R-3m(O3) in the discharged state. Such dynamic structural changes can adversely affect the stability of the crystal structure.

[0210] Furthermore, the two crystal structures that undergo dynamic structural changes also have a large difference in volume: When compared per the same number of cobalt atoms, the difference in volume between the H1-3 crystal structure and the discharged R-3m(O3) crystal structure is greater than 3.5%, typically 3.9% or more.

[0211] In addition, the H1-3 type crystal structure has CoO like the trigonal O1 type. 2 A structure with continuous layers is likely to be unstable.

[0212] Therefore, when charging and discharging are repeated so that x is 0.12 or less, the crystalline structure of conventional lithium cobalt oxide collapses. This collapse of the crystalline structure causes deterioration of cycle characteristics. This is because the collapse of the crystalline structure reduces the number of sites where lithium can exist stably and makes it difficult to insert and extract lithium. Note that not only when charging and discharging are repeated so that x is 0.12 or less, but also when x is 0.24 or less, collapse of the crystalline structure often occurs, causing deterioration of cycle characteristics. For this reason, in practical use, conventional lithium cobalt oxide is repeatedly charged and discharged in lithium-ion batteries while controlling x to a value greater than 0.24.

[0213] On the other hand, the positive electrode active material 10 shown in FIG. 4 that can be used as one embodiment of the present invention is Li x CoO 2 The change in the crystal structure between the discharged state where x is 1 and the state where x is 0.24 or less, or the state where x is 0.15, is smaller than that of conventional positive electrode active materials. Specifically, the positive electrode active material 10 has a smaller change in the crystal structure between the discharged state where x is 1 and the state where x is 0.24 or less, and a smaller change in the crystal structure of CoO 2 The layer misalignment can be reduced. Furthermore, the positive electrode active material 10 can reduce the change in volume per cobalt atom. Therefore, the positive electrode active material 10 is resistant to breakdown of its crystal structure even when repeatedly charged and discharged so that x is 0.24 or less, and can achieve excellent cycle characteristics. Furthermore, the positive electrode active material 10 has a low Li x CoO 2 When x is 0.24 or less, the positive electrode active material 10 can have a more stable crystal structure than conventional positive electrode active materials. x CoO 2 When the state where x is 0.24 or less is maintained, a short circuit is unlikely to occur, and the safety of the lithium ion battery is improved.

[0214] 4 shows the crystal structures of positive electrode active material 10 when x = 0.2 and x = 0.15, where 0.1 < x ≦ 0.24. When x = 0.2 and x = 0.15, positive electrode active material 10 has a crystal structure that differs from the H1-3 type crystal structure of conventional lithium cobalt oxide.

[0215] Specifically, when x=0.2, the positive electrode active material 10 has a crystal structure belonging to the trigonal space group R-3m. 2 The layer symmetry is the same as that of O3. For this reason, in this specification and the like, this crystal structure will be referred to as an "O3'-type crystal structure." In FIG. 4, R-3m(O3)' is added to the crystal structure where x = 0.2. Although the O3'-type crystal structure possessed by the positive electrode active material 10 has been described as a case where x = 0.2, if x is about 0.2, it can also be an O3'-type crystal structure. An x of about 0.2 can be expressed, for example, as 0.18≦x≦0.24, typically 0.18≦x≦0.22.

[0216] In the O3'-type crystal structure, the coordinates of cobalt and oxygen in the unit cell can be expressed in the range of Co(0,0,0.5), O(0,0,x), 0.20≦x≦0.25. The lattice constant a of the unit cell is preferably 0.2797≦a≦0.2837 (nm), more preferably 0.2807≦a≦0.2827 (nm), and typically a=0.2817 (nm). The lattice constant c is preferably 1.368≦c≦1.388 (nm), more preferably 1.375≦c≦1.381 (nm), and typically c=1.378 (nm).

[0217] As an example of 0.1<x≦0.24, when x=0.15, the positive electrode active material 10 has a crystal structure belonging to the monoclinic space group P2 / m. 2 There is one layer. For this reason, in this specification and the like, this crystal structure will be referred to as a "monoclinic O1(15) type crystal structure." In FIG. 4, the crystal structure with x = 0.15 is labeled P2 / m (monoclinic O1(15)). Although the monoclinic O1(15) type crystal structure of the positive electrode active material 10 has been described as a case where x = 0.15, if x is about 0.15, it can become a monoclinic O1(15) type crystal structure. An x of about 0.15 can be expressed, for example, as 0.13≦x≦0.24, typically 0.13≦x≦0.18.

[0218] The monoclinic O1(15) type crystal structure has the coordinates of cobalt and oxygen in the unit cell as Co1(0.5,0,0.5), Co2(0,0.5,0.5), O1(X O1 , 0, ZO1 ), 0.23≦X O1 ≦0.24, 0.61≦Z O1 ≦0.65, O2(X O2 , 0.5, Z O2 ), 0.75≦X O2 ≦0.78, 0.68≦Z O2 ≦0.71. The lattice constant a of the unit cell is a = 0.488 ± 0.001 (nm), the lattice constant b is b = 0.282 ± 0.001 (nm), and c = 0.484 ± 0.001 (nm). The angles indicating a monoclinic crystal are α = 90°, β = 109.58 ± 0.01°, and γ = 90°.

[0219] This crystal structure can also be fitted to the space group R-3m if a certain degree of error is allowed. In this case, the coordinates of the oxygen atoms of cobalt in the unit cell are Co(0,0,0.5), O(0,0,Z O ), 0.21≦Z O The lattice constant a of the unit cell is a=0.2817±0.002 (nm), and the lattice constant c is c=1.368±0.002 (nm).

[0220] In both the O3' and monoclinic O1(15) crystal structures, ions of cobalt, nickel, magnesium, etc. occupy six oxygen coordination positions, although light elements such as lithium may occupy four oxygen coordination positions.

[0221] As shown in FIG. 4, the R-3m(O3) in the discharged state, the O3′-type crystal structure, and the monoclinic O1(15)-type crystal structure show that CoO 2 There is almost no layer misalignment. The difference in volume per the same number of cobalt atoms between R-3m(O3) in a discharged state and the O3'-type crystal structure is 2.5% or less, more specifically 2.2% or less, and typically 1.8%. The difference in volume per the same number of cobalt atoms between R-3m(O3) in a discharged state and the monoclinic O1(15)-type crystal structure is 3.3% or less, more specifically 3.0% or less, and typically 2.5%.

[0222] The positive electrode active material 10 is Li x CoO 2It can be seen that when x is small, that is, when a large amount of lithium is released, the change in crystal structure is suppressed more than with conventional positive electrode active materials. Furthermore, the change in volume is also suppressed when compared per the same number of cobalt atoms. Therefore, it can be seen that the crystal structure of the positive electrode active material 10 is less likely to collapse even when repeatedly charged and discharged such that x is 0.24 or less, and the decrease in charge / discharge capacity during charge / discharge cycles is suppressed. Furthermore, because more lithium can be stably utilized than with conventional positive electrode active materials, the positive electrode active material 10 has a large discharge capacity per weight and per volume. Therefore, by using the positive electrode active material 10, a lithium-ion battery with a high discharge capacity per weight and per volume can be fabricated.

[0223] The positive electrode active material 10 is Li x CoO 2 It has been confirmed that when x is 0.15 or more and 0.24 or less, the O3' type crystal structure may be formed, and it is estimated that even when x is more than 0.24 and 0.27 or less, the O3' type crystal structure is formed. x CoO 2 It has been confirmed that when x is greater than 0.1 and less than 0.2, typically 0.13 or more and less than 0.18, the monoclinic O1(15) type crystal structure may be obtained. However, the crystal structure is similar to that of Li x CoO 2 The range of x is not necessarily limited to the above range, since it is affected not only by the x in the formula but also by the number of charge / discharge cycles, charge / discharge current, temperature, electrolyte, etc.

[0224] Therefore, the positive electrode active material 10 is Li x CoO 2 When x is greater than 0.1 and equal to or less than 0.24, the bulk portion 10b of the positive electrode active material 10 may have only the O3'-type crystal structure, only the monoclinic O1(15)-type crystal structure, or both. Furthermore, the bulk portion 10b of the positive electrode active material 10 does not necessarily have to have the O3'-type and / or the monoclinic O1(15)-type crystal structure. It may contain other crystal structures, or a portion may be amorphous.

[0225] Also, Li x CoO 2To make the value of x small, it is generally necessary to charge at a high charging voltage. x CoO 2 The state where x is small can be rephrased as a state charged at a high charging voltage. The positive electrode active material 10 is preferable because it can maintain the R-3m(O3) crystal structure even when charged at a high charging voltage, for example, a voltage of 4.6 V or higher at 25°C. The positive electrode active material 10 is also preferable because it can adopt an O3'-type crystal structure when charged at a higher charging voltage, for example, a voltage of 4.65 V or higher and 4.7 V or lower at 25°C. The positive electrode active material 10 is also preferable because it can adopt a monoclinic O1(15)-type crystal structure when charged at an even higher charging voltage, for example, a voltage of 4.7 V or higher and 4.8 V or lower at 25°C.

[0226] Even with positive electrode active material 10, if the charge voltage is further increased, H1-3 type crystals may finally be observed. Furthermore, as described above, since the crystal structure is affected by the number of charge / discharge cycles, charge / discharge current, electrolyte, etc., when the charge voltage is lower, for example, even if the charge voltage is 4.5 V or more and less than 4.6 V at 25° C., positive electrode active material 10 usable as one embodiment of the present invention may be able to adopt an O3′ type crystal structure. Similarly, when charged at a voltage of 4.65 V or more and 4.7 V or less at 25° C., it may be able to adopt a monoclinic O1(15) type crystal structure.

[0227] In addition, when graphite is used as the negative electrode active material in a lithium ion battery, the voltage of the lithium ion battery is lower than the above by the potential of the graphite. The potential of graphite is about 0.01 V to 0.7 V relative to the potential of lithium metal. Therefore, in the case of a lithium ion battery using graphite as the negative electrode active material, the same crystal structure is maintained at a voltage obtained by subtracting the potential of graphite from the above voltage.

[0228] In addition, although the O3'-type crystal structure and the monoclinic O1(15)-type crystal structure in Figure 4 are shown as having lithium present at all lithium sites with equal probability, this is not limited thereto. Lithium may be present disproportionately at some lithium sites. The distribution of lithium can be analyzed, for example, by neutron diffraction.

[0229] The O3' type crystal structure and the monoclinic O1(15) type crystal structure have random lithium between layers, but CdCl 2 It can be said that this crystal structure is similar to that of the CdCl type. 2 A similar crystal structure to the Li-type is lithium nickel oxide. 0.06 NiO 2 The crystal structure is similar to that when charged to 1000V, but pure lithium cobaltate or layered rock salt-type positive electrode active materials containing a large amount of cobalt usually have a CdCl 2 It is known that it does not have a typical crystal structure.

[0230] Furthermore, it is preferable that the concentration gradient of the additive element be the same at multiple locations on the surface layer 10a of the positive electrode active material 10. In other words, it is preferable that the reinforcement derived from the additive element is uniformly present in the surface layer 10a. Even if a portion of the surface layer 10a is reinforced, if there is a portion without reinforcement, stress may be concentrated in the unreinforced portion. If stress is concentrated in a portion of the positive electrode active material 10, defects such as cracks may occur there, which may lead to breakage of the positive electrode active material and a decrease in discharge capacity. However, it is not necessary for the additive element to have the same concentration gradient throughout the entire surface layer 10a of the positive electrode active material 10.

[0231] <Grain Boundaries> In addition to the distribution described above, it is more preferable that at least a portion of the additive elements contained in positive electrode active material 10 that can be used as one embodiment of the present invention is unevenly distributed in and near grain boundaries 11 as shown in FIG. 3B .

[0232] For example, the magnesium concentration at and near the grain boundaries 11 of the positive electrode active material 10 is preferably higher than that in other regions of the bulk portion 10b. The fluorine concentration at and near the grain boundaries 11 is also preferably higher than that in other regions of the bulk portion 10b. The nickel concentration at and near the grain boundaries 11 is also preferably higher than that in other regions of the bulk portion 10b. The aluminum concentration at and near the grain boundaries 11 is also preferably higher than that in other regions of the bulk portion 10b.

[0233] Since the grain boundaries 11 are one type of planar defect, they are prone to become unstable like the surface, and changes in the crystal structure are likely to begin at these boundaries. Therefore, by increasing the concentration of the added element at and near the grain boundaries 11, such changes in the crystal structure can be more effectively suppressed.

[0234] Furthermore, when the magnesium concentration and fluorine concentration are high at and near the grain boundaries 11, even if cracks occur along the grain boundaries 11 of the positive electrode active material 10 that can be used as one embodiment of the present invention, the magnesium concentration and fluorine concentration become high near the surface where the cracks occur. Therefore, the corrosion resistance to hydrofluoric acid can be improved even in the positive electrode active material after the cracks occur.

[0235] <Analysis method> In a certain positive electrode active material, Li x CoO 2 When x in the formula (I) is small, whether the positive electrode active material 10 has an O3′ type and / or a monoclinic O1(15) type crystal structure and can be used as one embodiment of the present invention can be determined by Li x CoO 2 This can be determined by analyzing a positive electrode having a positive electrode active material in a charged state in which x is small using XRD, electron beam diffraction, neutron diffraction, electron spin resonance (ESR), nuclear magnetic resonance (NMR), or the like.

[0236] In particular, XRD is preferred in that it can analyze the symmetry of transition metals such as cobalt contained in the positive electrode active material with high resolution, it can compare the level of crystallinity and the orientation of the crystals, it can analyze the periodic distortion of the lattice and the crystallite size, it can obtain sufficient accuracy even when measuring the positive electrode obtained by disassembling the lithium ion battery as it is, etc. Among XRD methods, powder XRD can obtain diffraction peaks that reflect the crystalline structure of the bulk portion 10b of the positive electrode active material 10, which occupies the majority of the volume of the positive electrode active material 10.

[0237] When the measurement sample is a powder, this is sometimes called the powder XRD measurement, and the powder can be set by placing it in a glass sample holder, sprinkling the sample on a greased silicone anti-reflection plate, etc. When the measurement sample is a positive electrode, the positive electrode can be attached to a substrate with double-sided tape, and the positive electrode active material layer can be set to match the measurement surface required by the device.

[0238] Furthermore, even in the case of cathode active material 10 that can be used as one embodiment of the present invention, if x is too small, such as 0.1 or less, or under conditions where the charging voltage exceeds 4.9 V, an H1-3 type or trigonal O1 type crystal structure may be formed. Therefore, to determine whether or not cathode active material 10 can be used as one embodiment of the present invention, analysis of the crystal structure, such as XRD, and information such as the charging capacity or the charging voltage are required.

[0239] Furthermore, when a positive electrode active material with a small x is exposed to the air, its crystal structure may change. For example, the crystal structure may change from O3'-type and monoclinic O1(15)-type to H1-3-type. Therefore, it is preferable to handle all samples used for crystal structure analysis in an inert atmosphere such as an argon atmosphere.

[0240] Furthermore, whether or not the distribution of the added elements contained in a certain positive electrode active material is in the state described above can be determined by analysis using, for example, XPS, energy dispersive X-ray spectroscopy (EDX), electron probe microanalysis (EPMA), or the like.

[0241] The crystal structure of the surface layer 10 a, the grain boundaries 11 and the like can be analyzed by electron beam diffraction or the like of a cross section of the positive electrode active material 10 .

[0242] <Evaluation Conditions> An example of an evaluation condition for determining whether a certain composite oxide is a cathode active material 10 that can be used as an embodiment of the present invention is to prepare a coin cell (e.g., CR2032 type, diameter 20 mm, height 3.2 mm) having lithium metal as a counter electrode and charge it under predetermined conditions. An example of an evaluation condition for determining whether a certain electrolyte is an electrolyte that can be used as an embodiment of the present invention is to prepare a coin cell (e.g., CR2032 type, diameter 20 mm, height 3.2 mm) having lithium metal as a counter electrode and charge it under predetermined conditions.

[0243] The procedure 1 described below is an example for confirming the physical properties of the positive electrode active material 10 that can be used as one embodiment of the present invention. Therefore, the electrolyte has a different configuration from that of the lithium ion battery that is one embodiment of the present invention.

[0244] Evaluation Procedure 1: A lithium-ion battery is disassembled, and the electrolyte-impregnated positive electrode is removed and punched out to a size that fits into a prepared coin cell. The positive electrode contains a conductive material and a binder in addition to the positive electrode active material. The electrolyte and other materials are removed before punching out the positive electrode. For example, after removing the positive electrode, the positive electrode can be washed using an organic solvent or the like.

[0245] The coin cell has lithium metal as the counter electrode. However, materials other than lithium metal can be used as the counter electrode. Unless otherwise specified, the potential in this specification is the potential of the positive electrode when the counter electrode is lithium metal.

[0246] The coin cell has a 25 μm thick porous polypropylene film as a separator.

[0247] The coin cell uses stainless steel (SUS) for the positive electrode can and stainless steel (SUS) for the negative electrode can.

[0248] In this way, a coin cell A for evaluation is prepared.

[0249] The coin cell A for evaluation prepared under the above conditions is subjected to constant current charging (also called CC charging) at a current value of 10 mA / g (equivalent to 0.05 C when 1 C is 200 mA / g of positive electrode active material weight) up to a desired voltage (e.g., 4.5 V, 4.55 V, 4.6 V, or 4.65 V, 4.7 V, 4.75 V, or 4.8 V). Charging at such a small current value is desirable for observing the phase change of the positive electrode active material.

[0250] The temperature during charging of the evaluation coin cell A can be 25° C. The temperature during charging may be the temperature of the thermostatic bath in which the coin cell A is placed.

[0251] After charging under these conditions, coin cell A is disassembled in a glove box under an argon atmosphere and the positive electrode is removed to obtain a positive electrode active material with a desired charge capacity. When various analyses are performed thereafter, it is preferable to seal the cell in an argon atmosphere to suppress reactions with external components. For example, XRD can be performed by sealing the cell in a sealed container under an argon atmosphere. Furthermore, it is preferable to remove and analyze the positive electrode promptly after charging is completed. Specifically, it is preferable to do so within one hour, and more preferably within 30 minutes, after charging is completed.

[0252] <Evaluation Procedure 2> A lithium-ion battery is disassembled, the positive electrode impregnated with the electrolyte is removed, and the electrolyte is analyzed by nuclear magnetic resonance (e.g. 1 Measurements using H NMR are performed to identify at least the organic solvent. Using nuclear magnetic resonance, the mixing ratio (volume ratio) of the organic solvent can also be identified. It is also possible to identify the lithium salt, additives, etc. contained in the electrolyte. Additives can also be added as long as they do not form a coating on the positive electrode active material, for example, materials for viscosity adjustment. In this case, the electrolyte may contain an additive.

[0253] The positive electrode is then punched out to a size that fits into a coin cell. The positive electrode contains a conductive material and a binder in addition to the positive electrode active material. The electrolyte and other components are removed after the nuclear magnetic resonance measurement but before punching out the positive electrode. For example, after removing the positive electrode, the positive electrode can be washed using an organic solvent or the like.

[0254] The coin cell has a lithium metal counter electrode, although other materials can also be used as the counter electrode.

[0255] The coin cell is prepared with an electrolyte identified by nuclear magnetic resonance spectroscopy, which is an embodiment of the present invention.

[0256] The coin cell has a 25 μm thick porous polypropylene film as a separator.

[0257] The coin cell uses stainless steel (SUS) for the positive electrode can and stainless steel (SUS) for the negative electrode can.

[0258] In this way, a coin cell B for evaluation is prepared.

[0259] The coin cell B for evaluation prepared under the above conditions is charged to a desired voltage (for example, 4.5 V, 4.55 V, 4.6 V, or 4.65 V, 4.7 V, 4.75 V, or 4.8 V) and then discharged. The following examples can be referenced for the charging conditions. The following examples can be referenced for the discharging conditions.

[0260] The temperature during charging of the evaluation coin cell B can be set to 25°C and below freezing, and it can be confirmed how the charge / discharge capacity at below freezing is compared to the charge / discharge capacity at 25°C.

[0261] <XRD> The XRD measurement performed on the coin cell A and the like can be performed using the following equipment and conditions. However, the equipment and conditions for the XRD measurement are not limited to those described below. XRD equipment: D8 ADVANCE manufactured by Bruker AXS X-ray source: CuKα 1 Line output: 40KV, 40mA

[0262] <Powder XRD pattern> CuKα calculated from the O3' type crystal structure, the monoclinic O1(15) type crystal structure, and the H1-3 type crystal structure model. 1 Ideal XRD patterns of the lines are shown in Figures 6, 7, 8A and 8B. x CoO 2 LiCoO where x=1 28A and 8B show the XRD patterns of the O3' type, the monoclinic O1(15) type and the H1-3 type, with Fig. 8A showing an enlarged view of the region in the 2θ (degree) range of 18° to 21°, and Fig. 8B showing an enlarged view of the region in the 2θ (degree) range of 42° to 46°. 2 (O3) and CoO 2 The pattern of (O1) was created using Reflex Powder Diffraction, a module of Materials Studio (BIOVIA), from crystal structure information obtained from ICSD (Inorganic Crystal Structure Database). The 2θ (degree) range was 15° to 75°, Step = 0.01°, and wavelength λ1 = 1.540562 × 10 −10 The monochromator was single. The pattern of the H1-3 type crystal structure was similarly created from the crystal structure information described in Non-Patent Document 2. The patterns of the O3' type and monoclinic O1(15) type crystal structures were estimated from the XRD pattern of a positive electrode active material usable as one embodiment of the present invention, and fitted using TOPAS ver. 3 (crystal structure analysis software manufactured by Bruker), and XRD patterns were created in the same manner as the others.

[0263] As shown in Figures 6, 8A, and 8B, when the O3' type crystal structure is analyzed by X-ray diffraction, diffraction peaks appear at 2θ (degrees) = 19.25 ± 0.12° (19.13° or more and less than 19.37°) and 2θ (degrees) = 45.47 ± 0.10° (45.37° or more and less than 45.57°).

[0264] Furthermore, in the monoclinic O1(15) type crystal structure, when analyzed by X-ray diffraction, diffraction peaks appear at 2θ (degrees) = 19.47 ± 0.10° (19.37° to 19.57°) and 2θ (degrees) = 45.62 ± 0.05° (45.57° to 45.67°).

[0265] On the other hand, as shown in Figures 7, 8A and 8B, no peaks appear at these positions in the H1-3 type crystal structure and trigonal O1. x CoO 2 The appearance of peaks at 19.13° or more and less than 19.37° and / or 19.37° or more and 19.57° or less, and at 45.37° or more and less than 45.57° and / or 45.57° or more and 45.67° or less when x is small can be said to be a characteristic of positive electrode active material 10 that can be used as one embodiment of the present invention.

[0266] It can also be said that the positions at which XRD diffraction peaks appear are close between the crystal structures where x = 1 and where x ≦ 0.24. More specifically, for the main diffraction peaks of the crystal structures where x = 1 and where x ≦ 0.24, which appear at 2θ (degrees) of 42° or more and 46° or less, the difference in 2θ (degrees) is 0.7° or less, more preferably 0.5° or less.

[0267] The positive electrode active material 10 that can be used in one embodiment of the present invention is Li x CoO 2 When x in the formula is small, the material has an O3'-type and / or monoclinic O1(15)-type crystal structure, but not all of the material has an O3'-type and / or monoclinic O1(15)-type crystal structure. It may contain other crystal structures, or a portion may be amorphous. However, when Rietveld analysis is performed on the XRD pattern, the O3'-type and / or monoclinic O1(15)-type crystal structure is preferably 50% or more, more preferably 60% or more, and even more preferably 66% or more. If the O3'-type and / or monoclinic O1(15)-type crystal structure is 50% or more, more preferably 60% or more, and even more preferably 66% or more, it can be a positive electrode active material with sufficiently excellent cycle characteristics.

[0268] Furthermore, even after 100 or more charge / discharge cycles from the start of measurement, when Rietveld analysis is performed, the O3' type and / or monoclinic O1(15) type crystal structure is preferably 35% or more, more preferably 40% or more, and even more preferably 43% or more.

[0269] Furthermore, the sharpness of the diffraction peaks in the XRD pattern indicates the degree of crystallinity. Therefore, it is preferable that each diffraction peak after charging is sharp, i.e., the half-width is narrow. The half-width varies depending on the XRD measurement conditions or the value of 2θ (degree), even for peaks arising from the same crystalline phase. In the case of the above-mentioned measurement conditions, for peaks observed at 2θ (degree) = 43° or more and 46° or less, the half-width is preferably 0.2° or less, more preferably 0.15° or less, and even more preferably 0.12° or less. Note that not all peaks necessarily meet this requirement. If some peaks meet this requirement, it can be said that the crystallinity of the crystalline phase is high. Therefore, it contributes to the stabilization of the crystalline structure after sufficient charging.

[0270] The crystallite size of the O3'-type and monoclinic O1(15) crystal structures of the positive electrode active material 10 is approximately equal to that of LiCoO 2 Therefore, even under the same XRD measurement conditions as the positive electrode before and after charging and discharging, the x CoO 2 When x in the graph is small, a clear peak of the O3' type crystal structure can be confirmed. 2 In this case, even if a part of the crystal structure resembles the O3'-type crystal structure, the crystallite size will be small and the peak will be broad and small. The crystallite size can be determined from the half-width of the XRD peak.

[0271] This embodiment mode can be freely combined with other embodiment modes.

[0272] Embodiment 3 In this embodiment, a configuration other than the positive electrode active material and the electrolyte contained in a lithium ion battery will be described.

[0273] [Positive Electrode] The positive electrode includes a positive electrode active material layer and a positive electrode current collector. The positive electrode active material layer includes a positive electrode active material and may further include at least one of a conductive additive and a binder. The positive electrode active material described in Embodiment 1 can be used.

[0274] FIG. 9A shows an example of a schematic cross-sectional view of a positive electrode.

[0275] The current collector 550 can be, for example, a metal foil. The positive electrode can be formed by applying a slurry to a metal foil and drying it. Note that pressing can also be performed after drying. The positive electrode is formed by forming an active material layer on the current collector 550.

[0276] The slurry is a material liquid used to form an active material layer on the current collector 550, and refers to a material containing an active material, a binder, and a solvent, and preferably further mixed with a conductive additive. The slurry is also called an electrode slurry or an active material slurry, and is sometimes called a positive electrode slurry when forming a positive electrode active material layer, and a negative electrode slurry when forming a negative electrode active material layer.

[0277] The positive electrode active material 561 has the function of taking in and / or releasing lithium ions during charging and discharging. The positive electrode active material 561 used in one embodiment of the present invention can be a material that exhibits little deterioration during charging and discharging, even at high charging voltages. Unless otherwise specified, the charging voltage is expressed based on the potential of lithium metal in this specification. Furthermore, in this specification, a high charging voltage is, for example, a charging voltage of 4.6 V or higher, preferably 4.65 V or higher, more preferably 4.7 V or higher, even more preferably 4.75 V or higher, and most preferably 4.8 V or higher.

[0278] The positive electrode active material 561 used in one embodiment of the present invention can be any material that does not deteriorate much due to charging and discharging even at a high charging voltage, and can be any material described in Embodiment 1 or 2. Note that the positive electrode active material 561 can be two or more materials with different particle sizes as long as the material does not deteriorate much due to charging and discharging even at a high charging voltage.

[0279] The conductive additive is also called a conductivity-imparting agent or a conductive material, and a carbon material can be used. By attaching the conductive additive between multiple active materials, the multiple active materials are electrically connected to each other, thereby increasing the conductivity. In this specification, the term "attachment" does not only refer to physical adhesion between the active material and the conductive additive, but also includes cases where a covalent bond is formed, bonding due to van der Waals forces, the conductive additive covers part of the surface of the active material, the conductive additive is embedded in the surface irregularities of the active material, and electrical connection even when not in contact with each other.

[0280] Specific examples of carbon materials that can be used as the conductive additive include carbon black (furnace black, acetylene black, graphite, etc.).

[0281] FIG. 9A illustrates carbon black 553 as a conductive additive.

[0282] A binder (resin) can be mixed to bond the current collector 550, such as a metal foil, and the active material to form the positive electrode of a lithium-ion battery. The binder is also called a binding agent. The binder is a polymeric material, and adding a large amount of binder reduces the proportion of active material in the positive electrode, thereby reducing the discharge capacity of the lithium-ion battery. Therefore, it is preferable to mix the minimum amount of binder. In Figure 9A, the areas not filled with the positive electrode active material 561, second active material 562, and carbon black 553 represent voids or binders.

[0283] 9A shows an example in which the positive electrode active material 561 is illustrated as a sphere, but this is not particularly limited. For example, the cross-sectional shape of the positive electrode active material 561 may be an ellipse, a rectangle, a trapezoid, a cone, a polygon with rounded corners, or an asymmetric shape. For example, FIG. 9B shows an example in which the positive electrode active material 561 has a polygonal shape with rounded corners.

[0284] 9B includes graphene 554 as a carbon material used as a conductive additive in the positive electrode. In FIG. 9B, a positive electrode active material layer including a positive electrode active material 561, graphene 554, and carbon black 553 is formed over a current collector 550.

[0285] In the step of mixing the graphene 554 and the carbon black 553 to obtain electrode slurry, the weight of the carbon black to be mixed is preferably 1.5 to 20 times, more preferably 2 to 9.5 times, that of the graphene.

[0286] Furthermore, when the mixture of graphene 554 and carbon black 553 is within the above range, the dispersion stability of carbon black 553 is excellent and agglomerations are less likely to occur during slurry preparation. Furthermore, when the mixture of graphene 554 and carbon black 553 is within the above range, a higher electrode density can be achieved than a positive electrode using only carbon black 553 as a conductive additive. Increasing the electrode density can increase the capacity per unit weight. Specifically, the density of the positive electrode active material layer measured gravimetrically can be 3.5 g / cc or more.

[0287] Although the electrode density is lower than that of a positive electrode using only graphene as a conductive additive, by mixing the first carbon material (graphene) and the second carbon material (acetylene black) within the above range, it is possible to accommodate rapid charging, and therefore it is particularly effective when used as an in-vehicle lithium-ion battery.

[0288] 9C illustrates an example of a positive electrode in which carbon fibers 555 are used instead of graphene. Fig. 9C shows an example different from Fig. 9B. The use of carbon fibers 555 can prevent aggregation of carbon black 553 and improve dispersibility.

[0289] In FIG. 9C, the regions not filled with the positive electrode active material 561, the carbon fibers 555, and the carbon black 553 indicate voids or binders.

[0290] 9D shows another example of a positive electrode. Fig. 9C shows an example in which carbon fiber 555 is used in addition to graphene 554. Using both graphene 554 and carbon fiber 555 can prevent aggregation of carbon black such as carbon black 553 and further improve dispersibility.

[0291] In FIG. 9D , regions that are not filled with the positive electrode active material 561 , the carbon fibers 555 , the graphene 554 , and the carbon black 553 indicate voids or binders.

[0292] A lithium-ion battery can be produced by using any one of the positive electrodes shown in Figures 9A to 9D, stacking a separator on the positive electrode, placing the stack of the negative electrode on the separator in a container (such as an outer casing or a metal can) that contains the stack, and filling the container with the electrolyte from the vesicles.

[0293] <Binder> As the binder, it is preferable to use a rubber material such as styrene-butadiene rubber (SBR), styrene-isoprene-styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, ethylene-propylene-diene copolymer, etc. Furthermore, as the binder, fluororubber can be used.

[0294] <Positive Electrode Current Collector> The current collector can be made of a highly conductive material, such as a metal such as stainless steel, gold, platinum, aluminum, or titanium, or an alloy thereof. It is preferable that the material used for the positive electrode current collector does not dissolve at the potential of the positive electrode. Aluminum alloys containing elements that improve heat resistance, such as silicon, titanium, neodymium, scandium, or molybdenum, can also be used. The current collector can also be made of a metal element that reacts with silicon to form a silicide. Examples of metal elements that react with silicon to form a silicide include zirconium, titanium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, cobalt, and nickel. The current collector can be in the form of a foil, plate, sheet, mesh, punched metal, expanded metal, or the like. The current collector should have a thickness of 5 μm to 30 μm.

[0295] [Negative Electrode] The negative electrode has a negative electrode active material layer and a negative electrode current collector. The negative electrode active material layer has a negative electrode active material, and may further have a conductive additive and a binder.

[0296] <Negative Electrode Active Material> As the negative electrode active material, for example, an alloy material and / or a carbon material can be used.

[0297] The negative electrode active material can be an element capable of undergoing a charge-discharge reaction through alloying and dealloying reactions with lithium. For example, one or more materials selected from silicon, tin, gallium, aluminum, germanium, lead, antimony, bismuth, silver, zinc, cadmium, indium, etc. can be used. These elements have a larger capacity than carbon, and silicon in particular has a high theoretical capacity of 4200 mAh / g. For this reason, it is preferable to use silicon as the negative electrode active material. Compounds containing these elements can also be used. For example, SiO, Mg 2 Si, Mg 2 Ge, SnO, SnO 2 , Mg 2 Sn, SnS 2 , V 2 Sn 3 , FeSn 2 , CoSn 2 , Ni 3 Sn 2 , Cu 6 Sn 5 , Ag 3 Sn, Ag 3 Sb, Ni 2 MnSb, CeSb 3 , LaSn 3 , La 3 Co 2 Sn 7 , CoSb 3 , InSb, SbSn, etc. Here, elements that can undergo charge-discharge reactions by alloying / dealloying reactions with lithium, and compounds containing such elements, are sometimes referred to as alloy-based materials.

[0298] In this specification, "SiO" refers to, for example, silicon monoxide. x Here, x preferably has a value of 1 or close to 1. For example, x is preferably 0.2 or more and 1.5 or less, and more preferably 0.3 or more and 1.2 or less.

[0299] The carbon material may be one or more selected from graphite, easily graphitizable carbon (soft carbon), non-graphitizable carbon (hard carbon), carbon fiber (carbon nanotube), graphene, carbon black, etc.

[0300] Examples of graphite include artificial graphite and natural graphite. Examples of artificial graphite include mesocarbon microbeads (MCMB), coke-based artificial graphite, and pitch-based artificial graphite. Here, spherical graphite having a spherical shape can be used as the artificial graphite. For example, MCMB may have a spherical shape and is therefore preferred. Furthermore, it is relatively easy to reduce the surface area of ​​MCMB, and this may be preferred. Examples of natural graphite include flake graphite and spherical natural graphite.

[0301] When lithium ions are inserted into graphite (when a lithium-graphite intercalation compound is formed), graphite exhibits a potential as low as that of metallic lithium (0.05 V to 0.3 V vs. Li / Li + This allows lithium-ion batteries using graphite to exhibit high operating voltages. Graphite is also preferred because it has advantages such as a relatively high capacity per unit volume, relatively small volume expansion, low cost, and greater safety compared to lithium metal.

[0302] Titanium dioxide (TiO 2 ), lithium titanium oxide (Li 4 Ti 5 O 12 ), lithium-graphite intercalation compound (Li x C 6 ), niobium pentoxide (Nb 2 O 5 ), tungsten oxide (WO 2 ), molybdenum oxide (MoO 2 ) and the like can be used.

[0303] In addition, as the negative electrode active material, a composite nitride of lithium and a transition metal, Li 3 Li with N-type structure 3−x M x N (M=Co, Ni, Cu) can be used. For example, Li 2.6 Co 0.4 N 3 has a large discharge capacity (900 mAh / g, 1890 mAh / cm 3 ) and is preferred.

[0304] When a composite nitride of lithium and a transition metal is used, lithium ions are contained in the negative electrode active material, so V, which does not contain lithium ions, can be used as the positive electrode active material. 2 O 5 , Cr 3 O 8 It is preferable that the composite nitride of lithium and a transition metal can be used as the negative electrode active material, even when a material containing lithium ions is used as the positive electrode active material, by first removing the lithium ions contained in the positive electrode active material.

[0305] In addition, a material that undergoes a conversion reaction can also be used as the negative electrode active material. For example, transition metal oxides that do not form an alloy with lithium, such as cobalt oxide (CoO), nickel oxide (NiO), and iron oxide (FeO), can also be used as the negative electrode active material. Further examples of materials that undergo a conversion reaction include Fe 2 O 3 , CuO, Cu 2 O, RuO 2 , Cr 2 O 3 oxides such as CoS 0.89 , sulfides such as NiS and CuS, Zn 3 N 2 , Cu 3 N, Ge 3 N 4 Nitrides such as NiP 2 , FeP 2 , CoP 3 Phosphides such as FeF 3 , BiF 3 This also occurs with fluorides such as

[0306] As the conductive additive and binder that can be contained in the negative electrode active material layer, the same materials as the conductive additive and binder that can be contained in the positive electrode active material layer can be used.

[0307] <Negative electrode current collector> The negative electrode current collector may be made of the same material as the positive electrode current collector, or may be made of copper, etc. It is preferable that the negative electrode current collector be made of a material that does not alloy with carrier ions such as lithium.

[0308] [Electrolyte] The electrolyte described in the first embodiment can be used.

[0309] [Separator] When the electrolyte contains a liquid electrolyte (also called an electrolyte solution), a separator is disposed between the positive electrode and the negative electrode. Examples of separators that can be used include cellulose-containing fibers such as paper, nonwoven fabrics, glass fibers, ceramics, or synthetic fibers such as nylon (polyamide), vinylon (polyvinyl alcohol-based fibers), polypropylene (referred to as PP), polyimide (referred to as PI), polyester, acrylic, polyolefin, and polyurethane. The porosity of the separator can be 35% to 90%, preferably 60% to 85%. Separators using polypropylene can have a porosity of 35% to 45%. Separators using polyimide can have a porosity of 75% to 85%. The separator thickness is preferably 10 μm to 80 μm, more preferably 20 μm to 60 μm. A separator using polyimide is preferable because it can have a high porosity and can be made thick (typically, the thickness is 50 μm or more and 60 μm or less).

[0310] The separator is preferably processed into a bag shape and disposed so as to encase either the positive electrode or the negative electrode.

[0311] The separator may have a multilayer structure. For example, an organic film such as polypropylene or polyethylene may be coated with a ceramic material, a fluorine-based material, a polyamide material, or a mixture of these. Examples of ceramic materials include aluminum oxide particles and silicon oxide particles. Examples of fluorine-based materials include PVDF and polytetrafluoroethylene. Examples of polyamide materials include nylon and aramid (meta-aramid, para-aramid).

[0312] By using a multilayer separator, the safety of the lithium-ion battery can be maintained even if the overall thickness of the separator is thin, and the capacity per volume of the lithium-ion battery can be increased.

[0313] [Exterior Body] The exterior body of a lithium-ion battery can be made of a metal material such as aluminum or a resin material. Alternatively, a film-like exterior body can be used. Examples of the film include a three-layer structure film in which a thin, flexible metal film such as aluminum, stainless steel, copper, or nickel is provided on a film made of a material such as polyethylene, polypropylene, polycarbonate, ionomer, or polyamide, and an insulating synthetic resin film such as a polyamide resin or polyester resin is further provided on the thin metal film as the outer surface of the exterior body.

[0314] This embodiment can be used in combination with other embodiments.

[0315] Embodiment 4 In this embodiment, an example of a lithium ion battery will be described.

[0316] [Laminated Lithium-ion Battery] An example of a laminated lithium-ion battery 100 is shown in FIGS. 10A and 10B . FIGS. 10A and 10B are external views, and the lithium-ion battery 100 includes the electrolyte and separator (not shown in FIG. 10 ) described in the above embodiment, a negative electrode 106, and a positive electrode 107. In the lithium-ion battery 100, the negative electrode 106 preferably has a larger area than the positive electrode 107. The lithium-ion battery 100 further includes a negative electrode lead electrode 510 electrically connected to the negative electrode 106 and a positive electrode lead electrode 511 electrically connected to the positive electrode 107. The electrolyte layer, the negative electrode 106, and the positive electrode 107 are housed in an outer casing 509, and a portion of the negative electrode lead electrode 510 and a portion of the positive electrode lead electrode 511 protrude from the outer casing 509. The outer casing 509 has an adhesive region 508 on a portion of its outer periphery. Fig. 10A shows an example in which the negative lead electrode 510 and the positive lead electrode 511 protrude from the same side of the exterior body 509, and the adhesive region 508 is located at least on the side from which each lead electrode protrudes and on two sides adjacent to that side. Fig. 10B shows an example in which the side from which the negative lead electrode 510 protrudes from the exterior body 509 and the side from which the positive lead electrode 511 protrudes from the exterior body 509 face each other, and the adhesive region 508 is located at least on the two sides from which each lead electrode protrudes and on one side sandwiched between those two sides. In Figs. 10A and 10B, the sides on which the adhesive region 508 is not located correspond to the folded sides of the exterior body 509.

[0317] When the organic solvent and positive electrode active material of the present invention are used in the laminated lithium ion battery 100, excellent charge / discharge characteristics are expected over a wide temperature range, including temperatures from below freezing to high temperatures.

[0318] [Coin-type lithium-ion battery] An example of a coin-type lithium-ion battery will be described. Fig. 11A is an exploded perspective view of a coin-type (single-layer flat) lithium-ion battery, Fig. 11B is an external view, and Fig. 11C is a cross-sectional view thereof. Coin-type lithium-ion batteries are mainly used in small electronic devices. In this specification, coin-type lithium-ion batteries include button-type lithium-ion batteries.

[0319] 11A is a schematic diagram that shows the overlapping of components (upper and lower relationships and positional relationships) for ease of understanding, and therefore, FIGS. 11A and 11B are not completely identical corresponding views.

[0320] 11A shows the state in which the positive electrode 304, negative electrode 307, spacer 342, and washer 332 are stacked and sealed with the negative electrode can 302 and positive electrode can 301. Note that the electrolyte and separator described in the above embodiment are not shown in FIG. 11A. The spacer 342 and washer 332 are used to protect the interior or fix the position within the can when the positive electrode can 301 and the negative electrode can 302 are crimped together. The spacer 342 or washer 332 is made of stainless steel or an insulating material.

[0321] A positive electrode 304 has a laminated structure in which a positive electrode active material layer 306 is formed on a positive electrode current collector 305 .

[0322] FIG. 11B is a perspective view of the completed coin-type lithium-ion battery 100.

[0323] In the coin-type lithium-ion battery 100, a positive electrode can 301, which also serves as a positive electrode terminal, and a negative electrode can 302, which also serves as a negative electrode terminal, may be insulated and sealed by a gasket 303 made of polypropylene or the like. The positive electrode 304 is formed by a positive electrode current collector 305 and a positive electrode active material layer 306 provided in contact with the positive electrode current collector. The negative electrode 307 is formed by a negative electrode current collector 308 and a negative electrode active material layer 309 provided in contact with the negative electrode current collector. The positive electrode can 301 is electrically connected to the positive electrode 304, and the negative electrode can 302 is electrically connected to the negative electrode 307.

[0324] In addition, the positive electrode 304 and the negative electrode 307 used in the coin-type lithium ion battery 100 each have an active material layer formed on only one surface.

[0325] As shown in FIG. 11C , the positive electrode can 301 is placed downward, and the positive electrode 304, the negative electrode 307, and the negative electrode can 302 are stacked in this order, and the positive electrode can 301 and the negative electrode can 302 are crimped together via a gasket 303 to produce a coin-shaped lithium ion battery 100.

[0326] When the organic solvent and positive electrode active material of the present invention are used in the coin-type lithium ion battery 100, excellent charge / discharge characteristics are expected over a wide temperature range, including temperatures from below freezing to high temperatures.

[0327] [Cylindrical Lithium-ion Battery] An example of a cylindrical lithium-ion battery will be described with reference to Fig. 12A. As shown in Fig. 12A, a cylindrical lithium-ion battery 616 has a positive electrode cap (battery lid) 601 on the top surface and a battery can (external can) 602 on the side and bottom surfaces. The positive electrode cap 601 and the battery can (external can) 602 are insulated by a gasket (insulating packing) 610.

[0328] Fig. 12B is a schematic diagram showing a cross section of a cylindrical lithium-ion battery. The cylindrical lithium-ion battery shown in Fig. 12B has a positive electrode cap (battery lid) 601 on the top surface and a battery can (external can) 602 on the side and bottom surfaces. The positive electrode cap and battery can (external can) 602 are insulated by a gasket (insulating packing) 610.

[0329] A battery element is provided inside a hollow cylindrical battery can 602, in which a strip-shaped positive electrode 604 and a negative electrode 606 are wound with an electrolyte layer 605 sandwiched therebetween. Although not shown, the battery element is wound around a central axis. One end of the battery can 602 is closed and the other end is open. Inside the battery can 602, the wound battery element, in which the positive electrode, the negative electrode, and the separator are wound, is sandwiched between a pair of opposing insulating plates 608 and 609. An electrolyte (not shown) of one embodiment of the present invention is injected into the battery can 602 in which the battery element is provided.

[0330] Since the positive and negative electrodes used in a cylindrical storage battery are wound, it is preferable to form active materials on both sides of the current collector. While the lithium-ion battery 616 shown in Figures 12A to 12D has a cylinder whose height is greater than its diameter, this is not limiting. A lithium-ion battery whose diameter is greater than its height may also be used. This configuration, for example, can reduce the size of the lithium-ion battery.

[0331] A positive electrode terminal (positive electrode current collector lead) 603 is connected to the positive electrode 604, and a negative electrode terminal (negative electrode current collector lead) 607 is connected to the negative electrode 606. Both the positive electrode terminal 603 and the negative electrode terminal 607 can be made of a metal material such as aluminum. The positive electrode terminal 603 is resistance-welded to a safety valve mechanism 613, and the negative electrode terminal 607 is resistance-welded to the bottom of the battery can 602. The safety valve mechanism 613 is electrically connected to the positive electrode cap 601 via a PTC (Positive Temperature Coefficient) element 611. The safety valve mechanism 613 cuts off the electrical connection between the positive electrode cap 601 and the positive electrode 604 when the increase in internal pressure of the battery exceeds a predetermined threshold. The PTC element 611 is a thermosensitive resistor whose resistance increases as the temperature increases, and the increased resistance limits the amount of current to prevent abnormal heat generation. The PTC element is made of barium titanate (BaTiO 3 )-based ceramic materials, etc. can be used.

[0332] 12C shows an example of a power storage system 615. The power storage system 615 has multiple lithium-ion batteries 616 and is sometimes called a battery pack. The positive electrodes of each lithium-ion battery are in contact with and electrically connected to conductors 624 separated by insulators 625. The conductors 624 are electrically connected to a control circuit 620 via wiring 623. The negative electrodes of each lithium-ion battery are electrically connected to the control circuit 620 via wiring 626. A protection circuit or the like that prevents overcharging or overdischarging can be used as the control circuit 620.

[0333] 12D shows an example of a power storage system 615. The power storage system 615 has a plurality of lithium ion batteries 616, which are sandwiched between a conductive plate 628 and a conductive plate 614. The plurality of lithium ion batteries 616 are electrically connected to the conductive plate 628 and the conductive plate 614 by wiring 627. The plurality of lithium ion batteries 616 may be connected in parallel, in series, or in parallel and then further connected in series. By configuring the power storage system 615 to have a plurality of lithium ion batteries 616, a large amount of power can be extracted.

[0334] A plurality of lithium ion batteries 616 may be connected in parallel and then further connected in series.

[0335] A temperature control device may be provided between the plurality of lithium ion batteries 616. When the lithium ion batteries 616 are overheated, they can be cooled by the temperature control device, and when the lithium ion batteries 616 are too cold, they can be heated by the temperature control device. This makes the performance of the power storage system 615 less susceptible to the influence of the outside air temperature.

[0336] 12D , the power storage system 615 is electrically connected to a control circuit 620 via wiring 621 and wiring 622. The wiring 621 is electrically connected to the positive electrodes of the plurality of lithium ion batteries 616 via a conductive plate 628, and the wiring 622 is electrically connected to the negative electrodes of the plurality of lithium ion batteries 616 via a conductive plate 614.

[0337] When the organic solvent and positive electrode active material of the present invention are used in a cylindrical lithium ion battery 100, excellent charge / discharge characteristics are expected over a wide temperature range, including temperatures from below freezing to high temperatures.

[0338] [Another Example of the Structure of the Lithium-Ion Battery] An example of the structure of the lithium-ion battery will be described with reference to FIGS. 13 and 14. FIG.

[0339] A lithium-ion battery 913 shown in FIG. 13A includes a wound body 950 in which terminals 951 and 952 are provided inside a housing 930. The wound body 950 is impregnated with the electrolyte of one embodiment of the present invention inside the housing 930. The terminal 952 is in contact with the housing 930, and the terminal 951 is not in contact with the housing 930 because an insulating material or the like is used. Note that for convenience, the housing 930 is shown separated in FIG. 13A , but in reality, the wound body 950 is covered by the housing 930, and the terminals 951 and 952 extend outside the housing 930. The housing 930 can be made of a metal material (for example, aluminum) or a resin material.

[0340] 13B, the housing 930 shown in Fig. 13A may be formed using a plurality of materials. For example, the lithium ion battery 913 shown in Fig. 13B has a housing 930a and a housing 930b bonded together, and a wound body 950 is provided in the area surrounded by the housing 930a and the housing 930b.

[0341] The housing 930a can be made of an insulating material such as organic resin. In particular, by using a material such as organic resin on the surface on which the antenna is formed, it is possible to prevent the lithium ion battery 913 from blocking the electric field. Note that if the electric field blocking by the housing 930a is small, the antenna may be provided inside the housing 930a. The housing 930b can be made of, for example, a metal material.

[0342] 13C shows the structure of the wound body 950. The wound body 950 has a negative electrode 931, a positive electrode 932, and an electrolyte layer 933. The wound body 950 is a wound body in which the negative electrode 931 and the positive electrode 932 are stacked on top of each other with the electrolyte layer 933 sandwiched therebetween, and the laminated sheet is wound. Note that multiple layers of the negative electrode 931, the positive electrode 932, and the electrolyte layer 933 may be stacked.

[0343] 14A to 14C , a lithium ion battery 913 having a wound body 950a can be provided. The wound body 950a shown in Fig. 14A includes a negative electrode 931, a positive electrode 932, and an electrolyte layer 933. The negative electrode 931 includes a negative electrode active material layer 931a. The positive electrode 932 includes a positive electrode active material layer 932a.

[0344] The electrolyte layer 933 has a width wider than the negative electrode active material layer 931 a and the positive electrode active material layer 932 a, and is wound so as to overlap the negative electrode active material layer 931 a and the positive electrode active material layer 932 a. From the standpoint of safety, it is preferable that the negative electrode active material layer 931 a be wider than the positive electrode active material layer 932 a. A wound body 950 a having such a shape is preferable due to its high safety and productivity.

[0345] 14B, the negative electrode 931 is electrically connected to a terminal 951. The terminal 951 is electrically connected to a terminal 911a. The positive electrode 932 is electrically connected to a terminal 952. The terminal 952 is electrically connected to a terminal 911b.

[0346] 14C , wound body 950a is covered with housing 930 to form lithium ion battery 913. Housing 930 is preferably provided with a safety valve, an overcurrent protection element, etc. The safety valve is a valve that opens when the inside of housing 930 reaches a predetermined internal pressure to prevent the battery from exploding.

[0347] As shown in Fig. 14B, the lithium ion battery 913 can be configured to have multiple wound bodies 950a. By using multiple wound bodies 950a, the lithium ion battery 913 can have a larger charge / discharge capacity. For other elements of the lithium ion battery 913 shown in Figs. 14A and 14B, the descriptions of the lithium ion battery 913 shown in Figs. 13A to 13C can be referred to.

[0348] When the organic solvent and positive electrode active material of the present invention are used in a lithium ion battery 913 having a wound body, excellent charge / discharge characteristics are expected over a wide temperature range, including temperatures from below freezing to high temperatures.

[0349] The content of this embodiment mode can be combined with the content of other embodiment modes as appropriate.

[0350] Fifth Embodiment In this embodiment, an example of application to an electric vehicle (EV) will be described with reference to FIG.

[0351] 15A , an electric vehicle is equipped with first batteries 1301 a and 1301 b as main driving lithium-ion batteries, and a second battery 1311 that supplies power to an inverter 1312 that starts a motor 1304. When the organic solvent and positive electrode active material of the present invention are used in first batteries 1301 a and 1301 b, excellent charge / discharge characteristics are expected over a wide temperature range, including temperatures from below freezing to high temperatures.

[0352] The second battery 1311 is also called a cranking battery (also called a starter battery). The second battery 1311 only needs to have high output, and does not need to have a large capacity, and the capacity of the second battery 1311 is smaller than that of the first batteries 1301a and 1301b.

[0353] The internal structure of the first battery 1301a may be a wound type or a stacked type. The first battery 1301a can use the secondary battery described in Embodiment 4. By using the secondary battery described in Embodiment 4 for the first battery 1301a, a high capacity can be achieved, safety can be improved, and the battery can be made smaller and lighter.

[0354] In this embodiment, an example is shown in which two first batteries 1301a and 1301b are connected in parallel, but three or more batteries may be connected in parallel. Furthermore, if the first battery 1301a can store sufficient power, the first battery 1301b may be omitted. By configuring a battery pack having multiple lithium ion batteries, it is possible to extract large amounts of power. The multiple lithium ion batteries may be connected in parallel, in series, or in series after being connected in parallel. A plurality of lithium ion batteries is also called a battery pack.

[0355] In addition, in an in-vehicle lithium-ion battery, in order to cut off power from multiple lithium-ion batteries, a service plug or circuit breaker that can cut off high voltage without using tools is provided in the first battery 1301a.

[0356] The power of the first batteries 1301a and 1301b is mainly used to rotate the motor 1304, but also supplies power to 42V in-vehicle components (such as an electric power steering 1307, a heater 1308, and a defogger 1309) via a DCDC circuit 1306. When a rear motor 1317 is provided for the rear wheels, the first battery 1301a is also used to rotate the rear motor 1317.

[0357] In addition, the second battery 1311 supplies power to 14V in-vehicle components (audio 1313, power windows 1314, lamps 1315, etc.) via the DCDC circuit 1310.

[0358] The first battery 1301a will be described with reference to FIG. 15B.

[0359] FIG. 15B shows an example in which nine prismatic lithium-ion batteries 1300 are combined into one battery pack 1415. Furthermore, nine prismatic lithium-ion batteries 1300 are connected in series, with one electrode fixed by a fixing portion 1413 made of an insulator and the other electrode fixed by a fixing portion 1414 made of an insulator. While this embodiment shows an example in which the batteries are fixed by the fixing portions 1413 and 1414, they may also be housed in a battery housing box (also called a casing). Because it is expected that a vehicle will be subjected to external vibrations or shaking (e.g., from the road surface), it is preferable to fix multiple lithium-ion batteries using the fixing portions 1413 and 1414 and the battery housing box. Furthermore, one electrode is electrically connected to the control circuit unit 1320 by wiring 1421. The other electrode is electrically connected to the control circuit unit 1320 by wiring 1422.

[0360] A memory circuit including a transistor using an oxide semiconductor can be used for the control circuit portion 1320. A charge control circuit or a battery control system including a memory circuit including a transistor using an oxide semiconductor may be referred to as a battery operating system (BTOS) or a battery oxide semiconductor (BTOS).

[0361] It is preferable to use a metal oxide that functions as an oxide semiconductor. For example, it is preferable to use a metal oxide such as In-M-Zn oxide (wherein the element M is one or more selected from aluminum, gallium, yttrium, copper, vanadium, beryllium, boron, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, and magnesium). In particular, the In-M-Zn oxide that can be used as the oxide is preferably a C-Axis Aligned Crystal Oxide Semiconductor (CAAC-OS) or a Cloud-Aligned Composite Oxide Semiconductor (CAC-OS). Furthermore, In—Ga oxide and In—Zn oxide can also be used as the oxide. A CAAC-OS is an oxide semiconductor having multiple crystalline regions, each with its c-axis aligned in a specific direction. The specific direction refers to the thickness direction of the CAAC-OS film, the normal direction to the surface where the CAAC-OS film is formed, or the normal direction to the surface of the CAAC-OS film. A crystalline region is a region with periodic atomic arrangement. If the atomic arrangement is considered as a lattice arrangement, a crystalline region is also a region with a uniform lattice arrangement. Furthermore, a CAAC-OS has a region where multiple crystalline regions are connected in the a-b plane direction, and the region may have distortion. Note that distortion refers to a portion where the lattice arrangement changes between a region with a uniform lattice arrangement and a region with another uniform lattice arrangement in a region where multiple crystalline regions are connected. In other words, a CAAC-OS is an oxide semiconductor with a c-axis aligned and no clear orientation in the a-b plane direction.

[0362] Furthermore, since the control circuit unit 1320 can be used in low-temperature environments, it is preferable to use a transistor using an oxide semiconductor. To simplify the process, the control circuit unit 1320 can also be formed using a unipolar transistor. Transistors using an oxide semiconductor for the semiconductor layer have a wider operating ambient temperature range than single-crystal Si, from −40° C. to 150° C., and their characteristics change less when the lithium-ion battery is heated than single-crystal Si. The off-current of a transistor using an oxide semiconductor is below the lower limit of measurement regardless of temperature, even at 150° C., whereas the off-current characteristics of single-crystal Si transistors are highly temperature-dependent. For example, at 150° C., the off-current of a single-crystal Si transistor increases, and the current on / off ratio does not become sufficiently large. The control circuit unit 1320 can improve safety.

[0363] The control circuit unit 1320, which uses a memory circuit including transistors using oxide semiconductors, can also function as an automatic control device for lithium-ion batteries to address 10 causes of instability, such as micro-short circuits. The functions for addressing the 10 causes of instability include overcharging prevention, overcurrent prevention, overheating control during charging, cell balancing in the battery pack, over-discharging prevention, a fuel gauge, automatic control of charging voltage and current according to temperature, control of charging current according to the degree of degradation, detection of abnormal behavior of micro-short circuits, and prediction of abnormalities related to micro-short circuits. The control circuit unit 1320 has at least one of these functions. Furthermore, the automatic control device for lithium-ion batteries can be miniaturized.

[0364] Micro-short circuits are tiny short circuits that occur inside lithium-ion batteries. One of the causes of micro-short circuits is said to be local current concentration in parts of the positive electrode and negative electrode due to uneven distribution of the positive electrode active material caused by multiple charge and discharge cycles, or the generation of by-products due to side reactions, which causes micro-short circuits.

[0365] In addition to detecting micro-short circuits, the control circuit 1320 can also be said to detect the terminal voltage of the lithium-ion battery and manage the charge / discharge state of the lithium-ion battery. For example, to prevent overcharging, it can turn off both the output transistor and the cutoff switch of the charging circuit almost simultaneously.

[0366] FIG. 15C shows an example of a block diagram of the battery pack 1415 shown in FIG. 15B.

[0367] The control circuit 1320 includes a switch unit 1324 including at least a switch for preventing overcharging and a switch for preventing overdischarging, a control circuit 1322 for controlling the switch unit 1324, and a voltage measurement unit for the first battery 1301a. The control circuit 1320 sets upper and lower voltage limits for the lithium-ion battery used and limits the upper limit of the external current and the upper limit of the output current. The range between the lower and upper voltage limits for the lithium-ion battery is within the recommended voltage range. When the voltage falls outside this range, the switch unit 1324 activates and functions as a protection circuit. The control circuit 1320 can also be called a protection circuit because it controls the switch unit 1324 to prevent overcharging and overdischarging. For example, if the control circuit 1322 detects a voltage that could cause overcharging, it turns off the switch unit 1324 to cut off the current. Furthermore, a PTC element can be provided in the charge / discharge path to provide a function for cutting off the current in response to an increase in temperature. The control circuit section 1320 also has an external terminal 1325 (+IN) and an external terminal 1326 (-IN).

[0368] The switch unit 1324 can be configured by combining an n-channel transistor and a p-channel transistor. The switch unit 1324 is not limited to a switch having a Si transistor using single crystal silicon, and may be, for example, Ge (germanium), SiGe (silicon germanium), GaAs (gallium arsenide), GaAlAs (gallium aluminum arsenide), InP (indium phosphide), SiC (silicon carbide), ZnSe (zinc selenide), GaN (gallium nitride), GaO xThe switch portion 1324 can also be formed using a power transistor having gallium oxide (x is a real number greater than 0). Furthermore, a memory element using an OS transistor can be freely arranged by stacking it on a circuit using a Si transistor, and thus integration can be easily achieved. By stacking the control circuit portion 1320 using an OS transistor on the switch portion 1324 and integrating them, it is possible to form it into a single chip, thereby enabling miniaturization.

[0369] The first batteries 1301a and 1301b mainly supply power to on-board equipment in the 42V system (high voltage system), while the second battery 1311 supplies power to on-board equipment in the 14V system (low voltage system). Lead-acid batteries are often used as the second battery 1311 due to their cost advantages. Using a lithium-ion battery as the second battery 1311 offers the advantage of being maintenance-free, but over long periods of use, such as three years or more, there is a risk of abnormalities occurring that cannot be detected at the time of manufacture. In particular, if the second battery 1311, which starts the inverter, becomes inoperable, even if the first batteries 1301a and 1301b have remaining capacity, the second battery 1311 is charged to maintain a full charge state by supplying power from the first battery to the second battery.

[0370] In this embodiment, an example in which lithium ion batteries are used for both the first battery 1301 a and the second battery 1311 is shown, but a lead-acid battery, an all-solid-state battery, or an electric double layer capacitor may also be used for the second battery 1311. When the organic solvent and the positive electrode active material of the present invention are used in the above-described lithium ion battery, excellent charge / discharge characteristics are expected in a wide temperature range including temperatures from below freezing to high temperatures.

[0371] Furthermore, regenerative energy generated by the rotation of the tire 1316 is sent to the motor 1304 via the gear 1305, and is then charged into the second battery 1311 from the motor controller 1303 and the battery controller 1302 via the control circuit unit 1321. Alternatively, the first battery 1301a is charged from the battery controller 1302 via the control circuit unit 1320. Alternatively, the first battery 1301b is charged from the battery controller 1302 via the control circuit unit 1320. In order to efficiently charge the regenerative energy, it is desirable that the first batteries 1301a and 1301b be capable of rapid charging.

[0372] The battery controller 1302 can set the charging voltage and charging current of the first batteries 1301a and 1301b. The battery controller 1302 can set charging conditions in accordance with the charging characteristics of the lithium ion batteries used, and can perform rapid charging.

[0373] Although not shown, when an external charger is connected, the charger's outlet or the charger's connection cable is electrically connected to the battery controller 1302. Power supplied from the external charger is charged to the first batteries 1301a, 1301b via the battery controller 1302. Some chargers are provided with a control circuit, and although the functions of the battery controller 1302 may not be used, it is preferable to charge the first batteries 1301a, 1301b via the control circuit unit 1320 to prevent overcharging. The control circuit unit 1320 may also be provided in the connection cable or the charger's connection cable. The control circuit unit 1320 is sometimes called an ECU (Electronic Control Unit). The ECU is connected to a CAN (Controller Area Network) provided in the electric vehicle. CAN is one of the serial communication standards used as an in-vehicle LAN. The ECU includes a microcomputer. The ECU uses a CPU or a GPU.

[0374] External chargers installed at charging stations and the like come in a variety of types, including 100V outlets, 200V outlets, and three-phase 200V and 50kW outlets. Charging can also be performed by receiving power from external charging equipment using a wireless power supply system or the like.

[0375] Next, an example in which a lithium-ion battery according to one embodiment of the present invention is mounted on a vehicle, typically a transportation vehicle, will be described.

[0376] Furthermore, installing lithium-ion batteries in vehicles will enable next-generation clean energy automobiles such as hybrid vehicles (HVs), electric vehicles (EVs), plug-in hybrid vehicles (PHVs), etc. Lithium-ion batteries can also be installed in transportation vehicles such as agricultural machinery, mopeds including electrically assisted bicycles, motorcycles, electric wheelchairs, electric carts, small or large ships, submarines, aircraft such as fixed-wing aircraft and rotary-wing aircraft, rockets, artificial satellites, space probes, planetary probes, and spacecraft.

[0377] 16A to 16D illustrate examples of transportation vehicles using one embodiment of the present invention. The automobile 2001 shown in FIG. 16A is an electric automobile that uses an electric motor as a power source for traveling. Alternatively, it is a hybrid automobile that can appropriately select and use an electric motor and an engine as a power source for traveling. When a lithium-ion battery is installed in a vehicle, an example of the lithium-ion battery described in the above embodiment is installed in one or more locations. When the organic solvent and the positive electrode active material of the present invention are used in a lithium-ion battery installed in a vehicle, excellent charge / discharge characteristics are expected over a wide temperature range, including temperatures from below freezing to high temperatures.

[0378] 16A includes a battery pack 2200, which includes a battery module to which a plurality of lithium-ion batteries are connected. The battery pack 2200 further preferably includes a charge control device electrically connected to the battery module.

[0379] Furthermore, the automobile 2001 can charge its lithium-ion battery by receiving power from an external charging facility using a plug-in system, a contactless power supply system, or the like. Charging can be performed using a predetermined charging method and connector standards, such as CHAdeMO (registered trademark) or Combo, as appropriate. The lithium-ion battery can be used in charging stations installed in commercial facilities and as a home power source. For example, plug-in technology can be used to charge an energy storage device installed in the automobile 2001 using an external power supply. Charging can be performed by converting AC power to DC power via a conversion device, such as an AC-DC converter.

[0380] Although not shown, a power receiving device can be mounted on a vehicle and power can be supplied contactlessly from a ground-based power transmitting device to charge the vehicle. In the case of this contactless power supply method, by incorporating a power transmitting device into a road or exterior wall, charging can be performed not only while the vehicle is stopped but also while the vehicle is moving. This contactless power supply method can also be used to transmit and receive power between two vehicles. Furthermore, solar cells can be installed on the exterior of the vehicle to charge the lithium-ion battery while the vehicle is stopped and while moving. Electromagnetic induction or magnetic resonance can be used for such contactless power supply.

[0381] Figure 16B shows a large transport vehicle 2002 having an electrically controlled motor as an example of a transport vehicle. The battery module of transport vehicle 2002 is, for example, a four-cell unit of lithium-ion batteries with a nominal voltage of 3.0 V to 5.0 V, with 48 cells connected in series to achieve a maximum voltage of 170 V. Other than the number of lithium-ion batteries in battery pack 2201, the battery pack 2201 has the same functions as those shown in Figure 15B, and therefore a description thereof will be omitted. When the organic solvent and positive electrode active material of the present invention are used in the lithium-ion batteries of battery pack 2201, excellent charge / discharge characteristics can be expected over a wide temperature range, including temperatures from below freezing to high temperatures.

[0382] 16C shows, as an example, a large transport vehicle 2003 having an electrically controlled motor. The battery module of the transport vehicle 2003 has, for example, one hundred or more lithium ion batteries with a nominal voltage of 3.0 V to 5.0 V connected in series to produce a maximum voltage of 600 V. Furthermore, except for the number of lithium ion batteries constituting the battery module of the battery pack 2202, the battery module has the same functions as that shown in FIG. 15B, and therefore a description thereof will be omitted. When the organic solvent and positive electrode active material of the present invention are used in the lithium ion batteries of the module, excellent charge / discharge characteristics can be expected over a wide temperature range, including temperatures from below freezing to high temperatures.

[0383] Fig. 16D shows, as an example, an aircraft 2004 having an engine that burns fuel. Since the aircraft 2004 shown in Fig. 16D has wheels for takeoff and landing, it can also be considered part of a transportation vehicle, and has a battery pack 2203 that includes a battery module formed by connecting multiple lithium-ion batteries and includes the battery module and a charge control device.

[0384] The battery module of the aircraft 2004 is, for example, eight 4 V lithium ion batteries connected in series, with a maximum voltage of 32 V. Other than the number of lithium ion batteries constituting the battery module of the battery pack 2203, the battery module has the same functions as those shown in FIG. 15B, and therefore a description thereof will be omitted.

[0385] The content of this embodiment mode can be combined with the content of other embodiment modes as appropriate.

[0386] Embodiment 6 In this embodiment, an example in which a lithium-ion battery according to one embodiment of the present invention is mounted on a vehicle such as a motorcycle or a bicycle will be described.

[0387] 17A illustrates an example of an electric bicycle using the lithium-ion battery of one embodiment of the present invention. The lithium-ion battery of one embodiment of the present invention can be applied to an electric bicycle 8700 illustrated in FIG. 17A. The lithium-ion battery of one embodiment of the present invention can also include a protection circuit.

[0388] The electric bicycle 8700 includes a power storage device 8702. The power storage device 8702 can supply electricity to a motor that assists a rider. The power storage device 8702 is portable and is shown in a state removed from the bicycle in FIG. 17B . The power storage device 8702 includes a plurality of lithium-ion batteries 8701 of one embodiment of the present invention, and the remaining battery charge and the like can be displayed on a display unit 8703. When the organic solvent and the positive electrode active material of the present invention are used in the lithium-ion battery 8701, excellent charge and discharge characteristics can be expected over a wide temperature range, including temperatures from below freezing to high temperatures.

[0389] The power storage device 8702 also includes a control circuit 8704 capable of controlling charging or detecting an abnormality of the lithium ion battery, an example of which is shown in Embodiment 7. The control circuit 8704 is electrically connected to the positive electrode and the negative electrode of the lithium ion battery 8701. This can greatly contribute to eliminating accidents such as fires caused by lithium ion batteries.

[0390] 17C illustrates an example of a two-wheeled vehicle using a lithium-ion battery of one embodiment of the present invention. A scooter 8600 illustrated in FIG. 17C includes a power storage device 8602, a side mirror 8601, and a turn signal light 8603. The power storage device 8602 can supply electricity to the turn signal light 8603. When the organic solvent and the positive electrode active material of the present invention are used in a lithium-ion battery, excellent charge and discharge characteristics can be expected over a wide temperature range, including temperatures from below freezing to high temperatures.

[0391] 17C can store a power storage device 8602 in an under-seat storage space 8604. The power storage device 8602 can be stored in the under-seat storage space 8604 even if the under-seat storage space 8604 is small.

[0392] The content of this embodiment mode can be combined with the content of other embodiment modes as appropriate.

[0393] Embodiment 7 In this embodiment, an example of mounting a lithium-ion battery according to one embodiment of the present invention in an electronic device will be described. Examples of electronic devices mounting a lithium-ion battery include television sets (also referred to as televisions or television receivers), computer monitors, digital cameras, digital video cameras, digital photo frames, mobile phones (also referred to as mobile phones or mobile phone devices), portable game consoles, personal digital assistants (PDAs), sound players, and large game consoles such as pachinko machines. Examples of personal digital assistants include notebook personal computers, tablet devices, e-book readers, and mobile phones.

[0394] 18A shows an example of a mobile phone. Mobile phone 2100 includes a display unit 2102 built into housing 2101, as well as operation buttons 2103, an external connection port 2104, a speaker 2105, a microphone 2106, and the like. Mobile phone 2100 also includes a lithium ion battery 2107. When the organic solvent and positive electrode active material of the present invention are used in a lithium ion battery, excellent charge / discharge characteristics can be expected over a wide temperature range, including temperatures from below freezing to high temperatures.

[0395] The mobile phone 2100 can execute various applications such as mobile phone calls, e-mail, document browsing and creation, music playback, internet communication, and computer games.

[0396] The operation button 2103 can be provided with various functions such as time setting, power on / off operation, wireless communication on / off operation, silent mode activation / deactivation, power saving mode activation / deactivation, etc. For example, the functions of the operation button 2103 can be freely set by an operating system incorporated in the mobile phone 2100.

[0397] The mobile phone 2100 is also capable of performing standardized short-range wireless communication, and can also make hands-free calls by communicating with a wirelessly enabled headset, for example.

[0398] The mobile phone 2100 also has an external connection port 2104, and can directly exchange data with other information terminals via a connector. Charging can also be performed via the external connection port 2104. Charging can also be performed by wireless power supply without using the external connection port 2104.

[0399] The mobile phone 2100 preferably has a sensor, such as a fingerprint sensor, a pulse sensor, a body temperature sensor, a touch sensor, a pressure sensor, an acceleration sensor, or the like.

[0400] FIG. 18B shows an unmanned aerial vehicle 2300 having multiple rotors 2302. The unmanned aerial vehicle 2300 is sometimes called a drone. The unmanned aerial vehicle 2300 includes a lithium-ion battery 2301 according to one embodiment of the present invention, a camera 2303, and an antenna (not shown). The unmanned aerial vehicle 2300 can be remotely controlled via the antenna. When the organic solvent and positive electrode active material of the present invention are used in a lithium-ion battery, excellent charge / discharge characteristics can be expected over a wide temperature range, including temperatures from below freezing to high temperatures.

[0401] Fig. 18C shows an example of a robot. A robot 6400 shown in Fig. 18C includes a lithium ion battery 6409, an illuminance sensor 6401, a microphone 6402, an upper camera 6403, a speaker 6404, a display unit 6405, a lower camera 6406, an obstacle sensor 6407, a movement mechanism 6408, a computing device, etc.

[0402] The microphone 6402 has a function of detecting the user's speaking voice, environmental sounds, etc. The speaker 6404 has a function of emitting sound. The robot 6400 can communicate with the user using the microphone 6402 and the speaker 6404.

[0403] The display unit 6405 has a function of displaying various information. The robot 6400 can display information desired by the user on the display unit 6405. The display unit 6405 can also be equipped with a touch panel. The display unit 6405 may also be a detachable information terminal, which can be installed in a fixed position on the robot 6400 to enable charging and data transfer.

[0404] The upper camera 6403 and the lower camera 6406 have the function of capturing images of the surroundings of the robot 6400. In addition, the obstacle sensor 6407 can detect the presence or absence of obstacles in the direction of travel when the robot 6400 moves forward using the movement mechanism 6408. The robot 6400 can recognize the surrounding environment and move safely using the upper camera 6403, the lower camera 6406, and the obstacle sensor 6407.

[0405] The robot 6400 includes a lithium-ion battery 6409 according to one embodiment of the present invention and a semiconductor device or electronic component in its internal region. When the organic solvent and the positive electrode active material of the present invention are used in the lithium-ion battery, excellent charge / discharge characteristics are expected over a wide temperature range, including temperatures from below freezing to high temperatures.

[0406] 18D shows an example of a cleaning robot. The cleaning robot 6300 includes a display unit 6302 arranged on the top surface of a housing 6301, a plurality of cameras 6303 arranged on the side surfaces, a brush 6304, an operation button 6305, a lithium-ion battery 6306, various sensors, and the like. Although not shown, the cleaning robot 6300 is provided with tires, a suction port, and the like. The cleaning robot 6300 can move by itself, detect dust 6310, and suck up the dust from a suction port arranged on the bottom surface.

[0407] For example, the cleaning robot 6300 can analyze an image captured by the camera 6303 and determine whether or not there is an obstacle such as a wall, furniture, or a step. Furthermore, if an object that may become entangled in the brush 6304, such as a wire, is detected through image analysis, the cleaning robot 6300 can stop the rotation of the brush 6304. The cleaning robot 6300 includes a lithium-ion battery 6306 according to one embodiment of the present invention and a semiconductor device or electronic component in its internal region. When the organic solvent and positive electrode active material of the present invention are used in the lithium-ion battery, excellent charge / discharge characteristics are expected over a wide temperature range, including temperatures from below freezing to high temperatures.

[0408] This embodiment mode can be implemented in appropriate combination with other embodiment modes.

[0409] Embodiment 8 In this embodiment, an example in which a lithium-ion battery according to one embodiment of the present invention is mounted on space equipment will be described.

[0410] 19A shows an artificial satellite 6800 as an example of space equipment. The artificial satellite 6800 has a body 6801, a solar panel 6802, an antenna 6803, and a lithium-ion battery 6805. The solar panel may be called a solar cell module.

[0411] When sunlight is irradiated onto the solar panel 6802, the power required for the operation of the satellite 6800 is generated. However, for example, in a situation where sunlight is not irradiated onto the solar panel or where the amount of sunlight irradiating the solar panel is low, the generated power is reduced. Therefore, the power required for the operation of the satellite 6800 may not be generated. In order to operate the satellite 6800 even under conditions where the generated power is low, it is preferable to provide a lithium ion battery 6805 in the satellite 6800. When the organic solvent and positive electrode active material of the present invention are used in a lithium ion battery, excellent charge / discharge characteristics can be expected over a wide temperature range, including temperatures from below freezing to high temperatures.

[0412] The satellite 6800 can generate a signal. The signal is transmitted via the antenna 6803, and can be received by, for example, a receiver installed on the ground or another satellite. By receiving the signal transmitted by the satellite 6800, the position of the receiver that received the signal can be measured, for example. As described above, the satellite 6800 can constitute, for example, a satellite positioning system.

[0413] Alternatively, the artificial satellite 6800 may be configured to include a sensor. For example, by including a visible light sensor, the artificial satellite 6800 may have the function of detecting sunlight reflected from an object on the ground. Alternatively, by including a thermal infrared sensor, the artificial satellite 6800 may have the function of detecting thermal infrared rays emitted from the earth's surface. As described above, the artificial satellite 6800 may function as, for example, an earth observation satellite.

[0414] FIG. 19B shows a probe 6900 equipped with a solar sail (also called a sun sail) as an example of space equipment. The probe 6900 includes a body 6901, a solar sail 6902, and a lithium-ion battery 6905. When the organic solvent and positive electrode active material of the present invention are used in the lithium-ion battery, excellent charge / discharge characteristics are expected over a wide temperature range, including temperatures from below freezing to high temperatures. When photons emitted from the sun strike the surface of the solar sail 6902, momentum is transferred to the solar sail 6902. Therefore, it is preferable that the surface of the solar sail 6902 be provided with a highly reflective thin film and be facing the sun.

[0415] The solar sail 6902 can also be designed to be folded up small until it leaves the atmosphere, and then deployed into a large sheet outside the Earth's atmosphere (outer space) as shown in Figure 19B.

[0416] FIG. 19C shows a spacecraft 6910 as an example of space equipment. The spacecraft 6910 has a body 6911, a solar panel 6912, and a lithium-ion battery 6913. When the organic solvent and positive electrode active material of the present invention are used in the lithium-ion battery, excellent charge / discharge characteristics can be expected over a wide temperature range, including temperatures from below freezing to high temperatures. The body 6911 can have, for example, a pressurized compartment and a non-pressurized compartment. The pressurized compartment can also be designed to accommodate a crew member. Electricity generated by sunlight irradiating the solar panel 6912 can be used to charge the lithium-ion battery 6913.

[0417] 19D shows a rover 6920 as an example of space equipment. The rover 6920 has a body 6921 and a lithium-ion battery 6923. When the organic solvent and positive electrode active material of the present invention are used in the lithium-ion battery, excellent charge / discharge characteristics are expected over a wide temperature range, including temperatures from below freezing to high temperatures. The rover 6920 may also be configured to have a solar panel 6922.

[0418] The rover 6920 may be configured to allow a crew member to ride in. The lithium ion battery 6923 may be charged with electricity generated by sunlight irradiating the solar panel 6912, or the lithium ion battery 6923 may be charged with electricity generated by other power sources, such as a fuel cell, a radioisotope thermoelectric converter, or the like.

[0419] The content of this embodiment mode can be combined with the content of other embodiment modes as appropriate.

[0420] In this example, a procedure for manufacturing a sample of an evaluation cell using a positive electrode active material of one embodiment of the present invention is described below.

[0421] <Production Conditions of Sample 1> The positive electrode active material of Sample 1 was LCO formed according to the solid phase method described in the second embodiment. The method for producing the LCO will be described. First, steps S11 to S13 in FIG. 2A are omitted, and the LiMO 2As the calcination material, lithium cobalt oxide (manufactured by Nippon Chemical Industry Co., Ltd., product name: C-10N, hereinafter referred to as "C-10N") was prepared. The median diameter (D50) of C-10N was approximately 12.0 μm. In step S15, the lithium cobalt oxide was placed in a sheath, which was then covered with a lid. The lithium cobalt oxide was then heated at 850° C. for 2 hours using a roller hearth kiln simulator furnace (manufactured by Noritake Company Ltd.) as a calcination furnace.

[0422] Air (compressed air, sufficiently dried) was flowed through the furnace at a rate of 10 L / min. Specifically, the opening width of the exhaust port was adjusted so that the furnace differential pressure gauge indicated 5 Pa. The furnace was cooled at a rate of 200°C / hour, and the air flow was not stopped until the temperature reached 200°C.

[0423] Next, as the A1 source in step S20_1, LiF and MgF are used as in step S21_1 of FIG. 2 LiF:MgF 2 In step S22_1, LiF and MgF were weighed out so that the molar ratio of LiF to MgF was 1:3 and the content was 1 atomic % relative to the lithium cobalt oxide, and the weighed out was sieved using an automatic sieving machine. 2 The above was mixed at a rotation speed of 500 rpm for 20 hours to prepare an additive element source (A1 source).

[0424] 2A, the Al source and the initially heated lithium cobalt oxide were dry-mixed using a Picobond (manufactured by Hosokawa Micron Co., Ltd.) at a rotation speed of 3000 rpm for 10 minutes, and then sieved using an automatic sieving machine to obtain a mixture 903 (step S32).

[0425] Next, in step S33, the mixture 903 was heated. The heating conditions were 900° C. and 20 hours. During heating, a lid was placed on the scabbard containing the mixture 903. By placing the lid, the inside of the scabbard was made into an oxygen-containing atmosphere, and the inflow and outflow of the oxygen could be blocked (O 2 A roller hearth kiln simulator furnace (manufactured by Noritake Co., Ltd.) was used as the firing furnace. Oxygen was flowed through the furnace at a rate of 10 L / min (O 2Specifically, the opening width of the exhaust port was adjusted so that the differential pressure gauge of the furnace was 5 Pa (positive pressure inside the furnace). When the furnace was cooled, it was cooled at a rate of 200°C / hour, and the oxygen flow was not stopped until the temperature reached 200°C. In this way, a composite oxide containing Mg and F was obtained.

[0426] Next, the A2 source in step S20_2 was prepared. 2 and Al(OH) 3 Each of these was weighed out so as to be 0.5 mol % relative to the lithium cobalt oxide, and then mixed while being crushed in dehydrated acetone as in step S22_2 to obtain a mixture A2, i.e., an A2 source. A Picobond (manufactured by Hosokawa Micron) was used as a mixing means, and the mixture was stirred at a rotation speed of 3000 rpm for 10 minutes to obtain a mixture A2 (step S23_2).

[0427] Thereafter, the mixture 903 and A2 were mixed as shown in step S34 of FIG. 2A, and the mixture 904 was obtained as shown in step S35. Next, as shown in step S36, the mixture 904 was heated at 850°C for 10 hours in a furnace into which oxygen was introduced. During heating, a lid was placed on the sachet containing the mixture 904. A roller hearth kiln simulator furnace (manufactured by Noritake Co., Ltd.) was used as the firing furnace, and the sachet was placed in the furnace and heated at the above heating temperature. Oxygen was flowed through the furnace at a rate of 10 L / min (O 2 The opening width of the exhaust port was adjusted so that the differential pressure gauge of the furnace was 5 Pa. The furnace was cooled at a rate of 200°C / hour, and the oxygen flow was not stopped until the temperature reached 200°C. In this way, lithium cobalt oxide containing Mg, F, Ni, and Al was obtained (step S37).

[0428] In this way, the positive electrode active material 10 of Sample 1 was obtained.

[0429] The positive electrode active material 10 of Sample 1 is an LCO containing Mg, F, Ni, and Al. x CoO 2 The change in the crystal structure between the discharge state where x is 1 and the state where x is 0.2 or 0.15 where x is 0.24 or less is smaller than that of conventional LCO.

[0430] <Preparation of Positive Electrode> Sample 1 was prepared as the positive electrode active material 10, acetylene black (AB) was prepared as the conductive material, and polyvinylidene fluoride (PVDF) was prepared as the binder. PVDF was prepared by dissolving it in N-methyl-2-pyrrolidone (NMP) at a weight ratio of 5%. Next, the positive electrode active material, AB, and PVDF were mixed in a weight ratio of 95:3:2 to prepare a slurry. NMP was used as the solvent for the slurry. The slurry was applied to an aluminum positive electrode current collector, and the solvent was then evaporated. The thickness of the aluminum positive electrode current collector was 20 μm.

[0431] Thereafter, in order to increase the density of the positive electrode active material layer, a pressing process was performed using a roll press machine after the solvent had evaporated. The pressing conditions were a linear pressure of 210 kN / m. The upper and lower rolls of the roll press machine were both set to 120°C. 120°C is the temperature at which PVDF melts. After pressing, the thickness of the positive electrode active material layer was 76 μm or more and 77 μm or less. The amount of the positive electrode supported was about 6 mg / cm. 2 It was decided.

[0432] Through the above steps, a positive electrode having Sample 1 was obtained.

[0433] A coin cell (CR2032 type, 20 mm diameter, 3.2 mm height) was assembled using Sample 1 as the positive electrode. The coin cell used lithium metal as the counter electrode. Stainless steel (SUS) was used for the positive and negative electrode cans of the coin cell. Such a coin cell is sometimes called a half cell or a test battery.

[0434] The coin cell of Sample 1 used PP as a separator. The coin cell of Sample 1 was not subjected to aging treatment. In this example, a secondary battery was completed without aging.

[0435] In this example, positive electrode active material 10 of Example 1 was used for the positive electrode, and cycle characteristics were evaluated for a half cell of Sample 1 of Example 1 using an electrolyte according to one embodiment of the present invention and a half cell of a comparative example.

[0436] <Conditions for preparing Sample 1> As the electrolyte for Sample 1, an organic solvent was prepared in which FEC:MTFP was mixed to satisfy a volume ratio of 2:8, and LiPF 5 was added as a lithium salt to the organic solvent at a concentration of 1 mol / L. 6 The electrolyte of Sample 1 is also called an F-substituted electrolyte.

[0437] The cycle characteristics were measured at environmental temperatures of 25° C. and 45° C. In this cycle test, 45° C. is included in the high temperature range.

[0438] The charging in the cycle test was performed by CC charging at a charge rate of 0.5 C until the end voltage reached 4.7 V, followed by CV charging until the current reached 0.05 C. A 10-minute rest period was held after the CV charging, and then discharge was initiated. CC discharging was performed at a discharge rate of 0.5 C until the end voltage reached 2.5 V. In this example, 1 C = 200 mA / g (current per weight of positive electrode active material: 200 mA / g). The results at an ambient temperature of 25°C are shown in FIG. 20A, and the results at 45°C are shown in FIG. 20B.

[0439] The above charge and discharge were counted as one cycle, and the number of cycles was repeated 50 times. The value calculated by (discharge capacity at the 50th cycle / maximum discharge capacity during the 50 cycles) × 100 was taken as the discharge capacity retention rate (%) at the 50th cycle. That is, a test was conducted in which 50 charge and discharge cycles were repeated, and the discharge capacity was measured for each cycle. The ratio of the discharge capacity measured at the 50th cycle to the maximum value of the discharge capacity during all 50 cycles (referred to as the maximum discharge capacity) was calculated and taken as the discharge capacity retention rate (%). A higher discharge capacity retention rate is desirable as a battery characteristic because it suppresses the decrease in battery capacity after repeated charge and discharge.

[0440] In the cycle test, the current is actually measured, and it is preferable to measure this current using the four-terminal method. During charging, electrons flow from the positive electrode terminal through the charge / discharge meter to the negative electrode terminal, so the charging current flows from the negative electrode terminal through the charge / discharge meter to the positive electrode terminal. During discharging, electrons flow from the negative electrode terminal through the charge / discharge meter to the positive electrode terminal, so the discharging current flows from the positive electrode terminal through the charge / discharge meter to the negative electrode terminal. The charging current and discharging current are measured by an ammeter included in the charge / discharge meter, and the integrated amounts of current flowing in one charge and one discharge correspond to the charge capacity and discharge capacity, respectively. For example, the integrated amount of discharge current flowing in the first discharge cycle can be referred to as the first cycle discharge capacity, and the integrated amount of discharge current flowing in the 50th discharge cycle can be referred to as the 50th cycle discharge capacity.

[0441] In addition, the charging in the cycle test was performed by CC charging at a charge rate of 0.5C until the end voltage reached 4.8V, followed by CV charging until the current reached 0.05C. A 10-minute rest period was held after CV charging, and then discharge was initiated. CC discharging was performed at a discharge rate of 0.5C until the end voltage reached 2.5V. In this example, 1C = 200mA / g (current per weight of positive electrode active material: 200mA / g). In this 4.8V cycle test, measurements were taken only at an ambient temperature of 25°C. The results are shown in Figure 21.

[0442] As an electrolyte for a comparative example, an organic solvent was prepared in which EC:DEC was mixed at a volume ratio of 3:7, and LiPF was added as a lithium salt to the organic solvent at a concentration of 1 mol / L. 6 The above-mentioned mixed solution was mixed with additive VC at a concentration of 2 wt %. The comparative example was the same as sample 1 except for the electrolyte. The results of the cycle test for the comparative example are shown in Figures 20A, 20B, and 21.

[0443] The discharge capacity at the first cycle, the maximum discharge capacity, and the rate of increase from the discharge capacity at the first cycle were also determined and are shown in Table 1 below.

[0444]

[0445] As shown in Table 1, Sample 1 had a high first-cycle discharge capacity, and the rate of increase from the first-cycle discharge capacity, i.e., the increase in capacity at the beginning of the cycle, was suppressed. At 25°C, the F-substituted electrolyte of Sample 1 showed an increase in capacity at the beginning of the cycle even without aging, but it was confirmed that the increase in capacity at the beginning of the cycle was suppressed more than in the comparative example. One of the reasons for this is thought to be that the F-substituted electrolyte, based on the results of impedance measurement, has significantly lower charge transfer resistance, etc., associated with solvation / desolvation of lithium ions or insertion / desorption of lithium ions into the positive electrode active material than other electrolytes.

[0446] The charge-discharge characteristics of Sample 1 are shown in Figure 22, with the vertical axis representing voltage and the horizontal axis representing capacity. Data from the first and tenth cycles are shown in Figure 22. As shown in Figure 22, Sample 1 exhibits high charge-discharge capacity from the early stages of cycling.

[0447] 23A shows a graph of Sample 1 with the capacity on the vertical axis and the cycle number on the horizontal axis, and Fig. 23B shows a graph of Sample 1 with the charge / discharge efficiency on the vertical axis and the cycle number on the horizontal axis. Note that the data from cycle number 1 to cycle number 10 in Fig. 23A are the same as those from cycle number 1 to cycle number 10 in Fig. 20A, and Fig. 23A corresponds to a partially enlarged view of Fig. 20A.

[0448] The results of the impedance measurements will be explained in the next example.

[0449] In this example, in order to measure AC impedance and evaluate charge / discharge characteristics, Sample 1_P and Reference Example 1 were prepared. The conditions for producing each sample will be described.

[0450] <Conditions for preparing Sample 1_P> As the electrolyte for Sample 1_P, an organic solvent mixed to satisfy FEC:MTFP=2:8 (volume ratio) was prepared, and lithium hexafluorophosphate (LiPF ) was added as a lithium salt to the organic solvent at a concentration of 1 mol / L. 6 ) was added. A solvent containing two or more organic solvents is sometimes called a mixed solvent. Note that no additive was used in Sample 1_P.

[0451] As the positive electrode active material of Sample 1_P, an LCO was used, which was formed according to a solid phase method in which a part of the manufacturing method of Embodiment 2 was modified. The manufacturing method of the LCO will be described. First, steps S11 to S13 in FIG. 2A are omitted, and the LiMO 2 As the Al source in step S20_1, lithium cobalt oxide (manufactured by Nippon Chemical Industry Co., Ltd., product name: C-10N, hereinafter referred to as "C-10N") was prepared. The median diameter (D50) of C-10N was approximately 12.0 μm. In step S15, the lithium cobalt oxide was heated at 850° C. for 2 hours in a furnace to which oxygen had been introduced. During heating, oxygen was not supplied to the furnace. Next, as in step S21_1 of FIG. 2B, LiF and MgF 2 LiF:MgF 2 LiF and MgF were weighed out so that the molar ratio of LiF to MgF was 1:3 and the content of MgF was 1 atomic % relative to the lithium cobalt oxide. 2 The Al source was obtained by mixing the Ni(OH) ions while grinding them. Then, in step S31 of FIG. 2A, the lithium cobalt oxide that had been heat-treated in step S15 was mixed with Al to obtain a mixture 903 as in step S32. In step S33, the mixture 903 was heated at 900°C for 20 hours in a furnace with oxygen introduced. During heating, oxygen was not supplied to the furnace. Next, the A2 source was prepared in step S20_2. Ni(OH) ions shown in step S21_2 of FIG. 2C were mixed with Al ions. 2 and Al(OH) 3 Each of these was weighed out to a concentration of 0.5 mol% relative to the lithium cobalt oxide, and then mixed while being crushed in dehydrated acetone as in step S22_2 to obtain mixture A2, i.e., A2 source. Then, mixture 903 and mixture A2 were mixed as in step S34 of FIG. 2A to obtain mixture 904 as in step S35. Next, in step S36, mixture 904 was heated at 850°C for 10 hours in a furnace with oxygen introduced. No oxygen was supplied to the furnace during heating. In this manner, the positive electrode active material of sample 1_P was obtained.

[0452] The positive electrode active material of Sample 1_P is LCO containing Mg, F, Ni, and Al, and the positive electrode active material is the above-mentioned Li xCoO 2 The change in the crystal structure between the discharge state where x is 1 and the state where x is 0.2 or 0.15 where x is 0.24 or less is smaller than that of conventional LCO.

[0453] The positive electrode of Sample 1_P was prepared using the above positive electrode active material, acetylene black (AB) as a conductive additive, and polyvinylidene fluoride (PVDF) as a binder. The PVDF was dissolved in N-methyl-2-pyrrolidone (NMP) as a solvent at a weight ratio of 5%. Next, a slurry containing the positive electrode active material, AB, and PVDF in a weight ratio of 95:3:2 was prepared, and the slurry was applied to an aluminum positive electrode current collector. The mixture was then pressed at a linear pressure of 210 kN / m and 120°C.

[0454] PP was used as the separator for Sample 1_P.

[0455] A coin cell (CR2032 type, diameter 20 mm, height 3.2 mm) was assembled using Sample 1_P as the positive electrode. The coin cell used lithium metal as the counter electrode. Stainless steel (SUS) was used for the positive and negative electrode cans of the coin cell.

[0456] <Production Conditions for Reference Example 1> As the electrolyte of Reference Example 1, an organic solvent mixed so as to satisfy EC:DEC=3:7 (volume ratio) was prepared, and LiPF 6 was added as a lithium salt to the organic solvent so as to have a concentration of 1 mol / L. 6 The above-mentioned mixed solution was mixed with additive VC at a concentration of 2 wt %. Reference Example 1 was the same as Sample 1_P except for the electrolyte described above.

[0457] <AC Impedance Measurement> The interfacial resistance between the positive electrode and the electrolyte was evaluated by an AC impedance method for Sample 1_P and Reference Example 1. The device used for the AC impedance measurement was a VMP3 (multi-Ch potentio / galvanostat) manufactured by Biologic.

[0458] First, using Sample 1_P as an example, the conditions for preparing an evaluation cell for AC impedance measurement will be described. An aging treatment was performed on a half cell having Sample 1_P. As the aging treatment, two cycles of charging under the following conditions and discharging under the following conditions were repeated. As the charging conditions, Sample 1_P was placed at an environmental temperature of 25°C, and constant current charging (hereinafter referred to as CC charging) was performed at a 0.1 C rate until the end voltage reached 4.6 V, followed by constant voltage charging (hereinafter referred to as CV charging) at 4.6 V until the current reached 0.01 C. As the discharging conditions, Sample 1_P was placed at an environmental temperature of 25°C, and constant current discharging (hereinafter referred to as CC discharging) was performed at a 0.1 C rate until the end voltage reached 2.5 V. As the aging treatment, a third charging cycle was then performed. As the charging conditions, Sample 1_P was placed at an environmental temperature of 25°C, and CC charging was performed at a 0.1 C rate until the end voltage reached 4.5 V, followed by CV charging until the current reached 0.01 C. The ambient temperature is the temperature of a thermostatic chamber (manufactured by Espec Corp.) in which each sample is placed, and will hereinafter be referred to simply as the ambient temperature. In this example, 1 C = 200 mA / g (current per weight of positive electrode active material is 200 mA / g).

[0459] After the third charging cycle, the half-cell containing Sample 1_P was left in a thermostatic chamber for 6 hours. Then, under an argon atmosphere, the positive electrode of Sample 1_P was removed from the half-cell. The removed positive electrode was impregnated with the electrolyte.

[0460] A symmetric cell was used as the evaluation cell for measuring AC impedance. Two removed positive electrodes were prepared, and a PP separator was placed between the two positive electrodes to assemble a symmetric cell. At this time, the amount of electrolyte in the symmetric cell was insufficient, so 1 mol / L LiPF was newly added to the cell to allow AC impedance evaluation. 6 An organic solvent containing FEC:MTFP=2:8 (volume ratio) was added. For Reference Example 1, a symmetric cell was assembled in the same manner as for Sample 1_P. In this manner, an evaluation cell for Sample 1 and an evaluation cell for Reference Example 1 were prepared.

[0461] Next, the conditions for measuring AC impedance will be explained. First, the Nyquist diagram and the equivalent circuit diagram used for fitting are shown in Figures 24A and 24B, respectively. In the Nyquist diagram of Figure 24A, Z' on the horizontal axis represents resistance [Ω], and -Z" on the vertical axis represents reactance [Ω]. In the equivalent circuit diagram of Figure 24B, CPE HF and CPE LF corresponds to the double layer capacitance. In Figures 24A and 24B, R S The resistance marked with corresponds to the resistance of the electrolyte, and R HF The resistance marked with R corresponds to the resistance related to the electron conduction in the electrode or the absorption and desorption of lithium ions on the electrode surface. LF The resistances marked with * correspond to the charge transfer resistance corresponding to the solvation and desolvation of lithium ions, the insertion and desorption of lithium ions, and the surface film resistance. The surface film can be formed by the decomposition of the organic solvent and its deposition on the active material. Note that W in Figures 24A and 24B is the diffusion coefficient corresponding to the diffusion of lithium ions in the solid.

[0462] The AC impedance measurements were performed using a measuring device combining a potentio / galvanostat (hereinafter referred to as "P / G") and a frequency response analyzer (hereinafter referred to as "FRA"), while controlling the environmental temperature in which the symmetric cell was placed to 25°C, 0°C, -20°C, -40°C, and 25°C, respectively. The FRA was set to an AC amplitude of 10 mV, and the frequency applied to the symmetric cell was varied between 0.3 mHz and 100 kHz. Specifically, the frequency was varied from 1 mHz to 100 kHz when the environmental temperatures were 25°C and 0°C, respectively.

[0463] FIG. 25A shows the results of measuring the AC impedance of Sample 1_P and Reference Example 1 when the ambient temperature was 25° C. LF The frequency at the apex of the arc corresponding to R was 3.8 Hz, and the resistance was 76 (Ω). LF The frequency at the apex of the arc corresponding to Z′ was 1.7 Hz, and the resistance was 126 (Ω). FIG. 25B shows an enlarged view of the boxed region in FIG. 25A where Z′ is near 50 (Ω). In sample 1_P, R HFThe frequency at the apex of the arc corresponding to R was 14094 Hz, and the resistance was 3.6 (Ω). HF The frequency at the apex of the arc corresponding to was 9520 Hz, and the resistance was 5.6 (Ω). S , R HF , R LF The following is a summary.

[0464] As can be seen from FIG. 25C, at an ambient temperature of 25° C., Sample 1_P has a higher R than Reference Example 1. LF In other words, since the separator material is common to Sample 1_P and Reference Example 1, Sample 1_P has a lower R than Reference Example 1 at an ambient temperature of 25°C. LF It can be said that the value of R LF As mentioned above, R is the charge transfer resistance corresponding to the solvation and desolvation of lithium ions, the insertion and desorption of lithium ions, and the surface film resistance component. LF It was speculated that because of the low charge-discharge current, a lithium ion battery having an electrolyte such as Sample 1_P would be able to achieve excellent charge-discharge characteristics over a wide temperature range, including temperatures from below freezing to high temperatures.

[0465] The AC impedance measurement conditions were as follows: an amplitude voltage of 10 mV, a frequency sweep ranging from 200 kHz to 10 mHz, and then an AC impedance value at 1001.6 Hz (sometimes referred to as 1 kHz) was extracted. During the sweep, 74 measurements were taken per digit. The measurement ambient temperature was 25°C. The lithium-ion secondary battery was charged to a voltage of 4.5 V, and then AC impedance measurement was performed within 2 hours. The results of the AC impedance measurement indicated that the lithium-ion secondary battery preferably had an impedance value of less than 90 mΩ at a frequency of 1 kHz after charging to a voltage of 4.5 V. The AC impedance measurement was performed immediately after charging the lithium-ion secondary battery to a voltage of 4.5 V. "Immediately after" refers to a period of 24 hours, preferably 12 hours, and more preferably 6 hours, between the end of charging the lithium-ion secondary battery and the start of AC impedance measurement.

[0466] 10a: surface layer portion, 10b: bulk portion, 10: positive electrode active material, 11: grain boundary, 100: lithium ion battery, 101: negative electrode current collector, 102: negative electrode active material layer, 104: positive electrode active material layer, 105: positive electrode current collector, 106: negative electrode, 107: positive electrode, 108: separator, 109: electrolyte, 301: positive electrode can, 302: negative electrode can, 303: gasket, 304: positive electrode, 305: positive electrode current collector, 306: positive electrode active material layer, 307: negative electrode, 308: negative electrode current collector, 309: negative electrode active material layer, 332: washer, 342: spacer, 508: adhesive region, 509: outer casing, 510: negative electrode lead lead electrode, 511: positive electrode lead electrode, 550: current collector, 553: carbon black, 554: graphene, 555: carbon fiber, 561: positive electrode active material, 562: second active material, 601: positive electrode cap, 602: battery can, 603: positive electrode terminal, 604: positive electrode, 605: electrolyte layer, 606: negative electrode, 607: negative electrode terminal, 608: insulating plate, 609: insulating plate, 611: PTC element, 613: safety valve mechanism, 614: conductive plate, 615: power storage system, 616: lithium ion battery, 620: control circuit, 621: wiring, 622: wiring, 623: wiring, 624: conductor, 625: insulator Insulator, 626: Wiring, 627: Wiring, 628: Conductive plate, 903: Mixture, 904: Mixture, 911a: Terminal, 911b: Terminal, 913: Lithium ion battery, 930a: Housing, 930b: Housing, 930: Housing, 931a: Negative electrode active material layer, 931: Negative electrode, 932a: Positive electrode active material layer, 932: Positive electrode, 933: Electrolyte layer, 950a: Wound body, 950: Wound body, 951: Terminal, 952: Terminal, 1300: Prismatic lithium ion battery, 1301a: First battery, 1301b: First battery, 1302: Battery controller, 1303: Motor controller, 1 304: motor, 1305: gear, 1306: DCDC circuit, 1307: electric power steering, 1308: heater, 1309: defogger, 1310: DCDC circuit, 1311: second battery, 1312: inverter, 1313: audio, 1314: power window, 1315: lamps, 1316: tires, 1317: rear motor, 1320: control circuit section, 1321: control circuit section, 1322: control circuit, 1324: switch section, 1413: fixed section, 1414: fixed section, 1415: battery pack, 1421: wiring, 1422: wiring, 2001: automobile,2002: Transport vehicle, 2003: Transport vehicle, 2004: Aircraft, 2100: Mobile phone, 2101: Housing, 2102: Display unit, 2103: Operation buttons, 2104: External connection port, 2105: Speaker, 2106: Microphone, 2107: Lithium ion battery, 2200: Battery pack, 2201: Battery pack, 2202: Battery pack, 2203: Battery pack, 2300: Unmanned aerial vehicle, 2301: Lithium ion battery, 2302: rotor, 2303: camera, 6300: cleaning robot, 6301: housing, 6302: display unit, 6303: camera, 6304: brush, 6305: operation button, 6306: lithium ion battery, 6310: dust, 6400: robot, 6401: illuminance sensor, 6402: microphone, 6403: upper camera, 6404: speaker, 6405: display unit, 6406: Lower camera, 6407: Obstacle sensor, 6408: Moving mechanism, 6409: Lithium ion battery, 6800: Satellite, 6801: Airframe, 6802: Solar panel, 6803: Antenna, 6805: Lithium ion battery, 6900: Probe, 6901: Airframe, 6902: Solar sail, 6905: Lithium ion battery, 6910: Spacecraft, 6911: Airframe, 6912: Solar -panel, 6913: lithium ion battery, 6920: rover, 6921: fuselage, 6922: solar panel, 6923: lithium ion battery, 8600: scooter, 8601: side mirror, 8602: power storage device, 8603: turn signal light, 8604: under-seat storage, 8700: electric bicycle, 8701: lithium ion battery, 8702: power storage device, 8703: display unit, 8704: control circuit,

Claims

The battery includes a positive electrode having a positive electrode active material and an electrolyte, The positive electrode active material includes lithium cobalt oxide containing magnesium, the magnesium concentration in the surface layer portion of the positive electrode active material is higher than the magnesium concentration in the interior of the positive electrode active material, The lithium ion secondary battery, wherein the electrolyte contains a fluorinated cyclic carbonate and a fluorinated chain carbonate.

2. The lithium ion secondary battery according to claim 1, wherein the positive electrode active material is lithium cobalt oxide further containing aluminum, nickel, and fluorine.

2. The lithium ion secondary battery according to claim 1, wherein when the lithium ion secondary battery is charged to a voltage of 4.5 V and then AC impedance measurement is performed, the result satisfies less than 90 mΩ at a frequency of 1 kHz.

2. The lithium ion secondary battery of claim 1, wherein the lithium cobalt oxide is in contact with the electrolyte.

Citation Information

Patent Citations

  • Nonaqueous electrolyte solution for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, and method for manufacturing nonaqueous electrolyte secondary battery

    JP2017208246A

  • Negative electrode for nonaqueous electrolyte power storage device, nonaqueous electrolyte power storage element, and their manufacturing method

    JP2022180183A

  • Method for manufacturing lithium-ion secondary batteries

    JP2023033572A

  • Non-aqueous electrolyte secondary cell

    WO2018123238A1

  • Secondary battery and electronic device

    WO2022229776A1