Horizontal polymerization reactor for producing propylene polymer and method for producing propylene polymer
The horizontal polymerization reactor design addresses the accumulation of fine propylene polymer powder by using a partitioned compartment and controlled purge gas flow, ensuring operational stability and preventing equipment damage through effective management of the pressure equalization line.
Patent Information
- Application Number
- PCT/JP2023/013371
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-03
AI Technical Summary
Horizontal polymerization reactors face issues with fine propylene polymer powder accumulating at the sliding interface between the stirring shaft and the bearing, leading to increased frictional load, instability of the polymerization reaction, and equipment deterioration due to blockage of the pressure equalization line during long-term operation.
A horizontal polymerization reactor design with a cylindrical reaction vessel, a stirrer rotating in the circumferential direction, and a partition wall separating the reaction chamber from the bearing compartment, along with a pressure equalization line and purge gas supply line, where the distance from the catalyst supply nozzle to the pressure equalization line is set at 10% of the reaction chamber length, and the purge gas flow rate is maintained at 0.2 m/sec or more to prevent fine powder intrusion.
This design prevents partition wall damage and maintains operational stability by reducing the accumulation of fine powder in the pressure equalization line, thus preventing blockage and maintaining the stability of the polymerization reaction and stirring performance.
Smart Images

Figure JP2023013371_03102024_PF_FP_ABST
Abstract
Description
Horizontal polymerization reactor for producing propylene polymers and method for producing propylene polymers
[0001] The present invention relates to a horizontal polymerization reactor used for producing a propylene polymer, and a method for producing a propylene polymer using the polymerization reactor.
[0002] Propylene-based polymers, including propylene homopolymers and propylene copolymers, have excellent mechanical properties such as rigidity and heat resistance, good moldability, can be produced relatively inexpensively, and are highly environmentally friendly, and therefore are widely used in industrial applications.
[0003] In the production process of propylene-based polymers, when industrial production of propylene-based polymers began, catalyst performance was low, and a step of removing catalyst residues, atactic polymers, etc. from the obtained propylene-based polymers was necessary, and processes such as a slurry method using a solvent were mainly used. Subsequently, as catalyst performance has improved dramatically, the necessity of removing catalyst residues, atactic polymers, etc. has decreased, and currently gas-phase polymerization methods have become the mainstream process.
[0004] Known gas-phase polymerization reactors for olefins such as propylene and ethylene include a reactor vessel, which is the main body of the polymerization reactor, and an agitator having a stirring shaft and a stirring blade fixed on the stirring shaft, which is disposed within the reactor vessel as a means for homogenizing a reaction system containing raw material monomers and a catalyst. Patent Document 1 discloses a so-called vertical polymerization reactor in which a cylindrical reactor vessel is installed vertically and an agitator having a stirring shaft that rotates about a vertical axis is disposed within the reactor. Patent Document 2 discloses a so-called horizontal polymerization reactor in which a cylindrical reactor vessel is installed horizontally and an agitator having a stirring shaft that rotates about a horizontal axis is disposed within the reactor.
[0005] When a propylene polymer is produced by gas-phase polymerization using a horizontal polymerization reactor, a catalyst is generally supplied to the upstream region of the reactor. The catalyst is in the form of fine particles, and propylene polymerizes on the surface and inside of the catalyst fine particles to form propylene polymer particles. The propylene polymer particles grow as the polymerization proceeds and gradually move downstream of the reactor, and the grown propylene polymer powder is removed from the downstream side of the reactor. Therefore, around the catalyst supply zone in the upstream region of the reactor, there is a high probability that the catalyst fine particles supplied to the reactor and propylene polymer particles with small particle sizes (hereinafter, both will be collectively referred to as "propylene polymer fine powder" or simply "fine powder") will be present. Such fine powder penetrates into the sliding interface between the stirring shaft of the stirrer and the inner surface of the bearing, causing problems in the production process. When fine powder of the propylene polymer accumulates at the sliding interface between the stirring shaft and the inner surface of the bearing, a large frictional load is generated. This frictional load causes deterioration of stirring performance, such as a decrease in the smoothness and stability of stirring, and can also cause damage to the stirring shaft or the bearing. Ultimately, this can lead to problems such as a loss of stability of the polymerization reaction in the polymerization reactor, ease of maintenance of the apparatus, and durability of the entire apparatus.
[0006] JP-A-53-123487 JP-A-63-223001
[0007] The present inventors have designed a horizontal polymerization reactor having the following features for the purpose of producing a propylene polymer by gas-phase polymerization. (1) The horizontal polymerization reactor is equipped with a horizontally installed cylindrical reaction vessel, an agitator having an agitator shaft that rotates circumferentially around the body of the reaction vessel, and an agitator having an agitator fixed on the agitator shaft. (2) A partition wall is provided at one end of the interior space of the reaction vessel, and the partition wall divides the interior space of the reaction vessel into a reaction chamber where the polymerization reaction takes place and a bearing compartment adjacent to the reaction chamber, and a bearing for the agitator is housed in the bearing compartment. (3) The agitator shaft is positioned in the reaction chamber in alignment with the central axis extending in the longitudinal direction of the reaction vessel, and one end of the agitator shaft penetrates the partition wall from the reaction chamber into the bearing compartment, and the agitator shaft is supported by a bearing in the bearing compartment so as to be rotatable about its axis. (4) The reaction chamber and the bearing compartment are connected via a pressure equalizing line that serves as a gas flow path. (5) A purge gas supply line is connected to the pressure equalization line, and gas is purged from the purge gas supply line to the pressure equalization line.
[0008] The horizontal polymerization reactor having the above-mentioned features has the following improvements: (1) Since the bearings are housed in the bearing compartment of the reaction vessel, the risk of fluid leakage from the reaction vessel to the outside can be reduced compared to when the bearings are installed outside the reaction vessel. (2) The bearings in the bearing compartment are protected from exposure to fine particles present in the reaction chamber by the partition wall separating the reaction chamber and the bearing compartment, so the bearings can be kept clean. (3) By providing a pressure equalization line between the reaction chamber and the bearing compartment, a pressure equalization state between the reaction chamber and the bearing compartment can be maintained, preventing damage to the partition wall due to the pressure difference between the reaction chamber and the bearing compartment, and the intrusion of fine particles from the reaction chamber into the bearing compartment can be reduced by the effect of gas purging to the pressure equalization line.
[0009] However, the present inventors have confirmed that simply providing a pressure equalization line in a horizontal polymerization reactor, connecting a purge gas supply line to the pressure equalization line, and purging the pressure equalization line with gas is not effective enough to prevent fine particles from entering the pressure equalization line from the reaction chamber and further into the bearing compartment, and that during long-term operation of the polymerization reactor, fine particles gradually accumulate in the pressure equalization line, the bearing compartment, and at the sliding interface between the agitator shaft and the inner surface of the bearing, causing destabilization of the polymerization reaction due to blockage of the pressure equalization line and deterioration of stirring performance due to increased frictional load at the sliding interface between the agitator shaft and the inner surface of the bearing.
[0010] In view of the problems faced by horizontal polymerization reactors designed as described above, the present invention aims to provide a horizontal polymerization reactor for producing a propylene polymer by gas phase polymerization, which not only does not suffer from partition wall damage during long-term operation but also has operational stability that is less susceptible to problems such as destabilization of the polymerization reaction due to clogging of the pressure equalizing line during long-term operation and deterioration of stirring performance due to increased friction load at the sliding interface between the stirring shaft and the inner surface of the bearing. Another object of the present invention is to provide a method for producing a propylene polymer using the polymerization reactor having such high long-term operational stability.
[0011] As a result of extensive investigations into solving the above problems, the present inventors have found that, in a horizontal polymerization reactor for producing a propylene polymer by gas phase polymerization, by providing a pressure equalization line between the reaction chamber and the bearing compartment, and further setting the longitudinal distance of the polymerization reactor from the connection position between the polymerization reaction chamber and the catalyst feed nozzle to the connection position between the polymerization reaction chamber and the pressure equalization line to a length that is at least a certain percentage of the entire length of the polymerization reaction chamber, an increase in the pressure difference between the reaction chamber and the bearing compartment due to clogging of the pressure equalization line during long-term operation, and a deterioration in stirring performance due to an increase in frictional load at the sliding interface between the stirring shaft and the inner surface of the bearing, can be made less likely to occur.
[0012] A first aspect of the present invention is a horizontal polymerization reactor for producing a propylene-based polymer, comprising: a cylindrical reactor body having an internal space and a polymerization reaction chamber and a bearing chamber separated by a partition wall that crosses the longitudinal direction of the internal space; an agitator having an agitator shaft that rotates in the circumferential direction of the reactor body and an agitator part fixed on the agitator shaft; a bearing that is disposed on at least one end of the agitator shaft and receives an end of the agitator shaft; a pressure equalizing line connecting the polymerization reaction chamber and the bearing chamber; a purge gas supply line connected to at least the pressure equalizing line; and a catalyst supply nozzle that is connected to a catalyst supply port of the polymerization reaction chamber; wherein the agitator shaft penetrates the partition wall and is housed in the polymerization reaction chamber and the bearing chamber, the agitator part is housed in the polymerization reaction chamber, and the bearing is housed in the bearing chamber, the distance in the longitudinal direction of the polymerization reactor from a position where the catalyst supply port of the polymerization reaction chamber is connected to the catalyst supply nozzle to a position where the polymerization reaction chamber is connected to the pressure equalizing line is 10% or more of the length of the polymerization reaction chamber.
[0013] In the horizontal polymerization reactor of the first invention, it is preferable that the cross-sectional area of the flow path of the pressure equalizing line be such that a cross-sectional area (IA1) of the flow path at a connection portion between the pressure equalizing line and the polymerization reaction chamber and a cross-sectional area (IA2) of the flow path at a connection portion between the pressure equalizing line and the purge gas supply line satisfy the relationship expressed by the following formula: IA1<IA2.
[0014] A second aspect of the present invention is a method for producing a propylene-based polymer, which comprises polymerizing a monomer containing propylene using the horizontal polymerization reactor of the first aspect of the present invention.
[0015] In the method for producing a propylene-based polymer according to the second aspect of the present invention, the flow rate (FR1) of the purge gas at a junction between the pressure equalizing line and the polymerization reaction chamber in a direction toward the polymerization reaction chamber and the flow rate (FR2) of the purge gas at a junction between the pressure equalizing line and the purge gas supply line in a direction toward the polymerization reaction chamber preferably satisfy the relationship represented by the following formula: FR1>FR2.
[0016] In the second aspect of the present invention, the method for producing a propylene polymer preferably has a flow rate (FR1) of 0.2 m / sec or more in the direction toward the polymerization reaction chamber at the connecting portion between the pressure equalization line and the polymerization reaction chamber.
[0017] In the method for producing a propylene-based polymer according to the second aspect of the present invention, it is preferable to use a purge gas containing propylene.
[0018] According to the present invention, there is provided a horizontal polymerization reactor for producing a propylene polymer by a gas phase polymerization method, which not only does not suffer from partition wall damage during long-term operation but also has operational stability that is less susceptible to problems such as destabilization of the polymerization reaction due to clogging of the pressure equalization line during long-term operation and deterioration of stirring performance due to increased friction load at the sliding interface between the stirring shaft and the inner surface of the bearing. Furthermore, according to the present invention, there is provided a method for producing a propylene polymer using the above-mentioned polymerization reactor having high long-term operational stability.
[0019] Fig. 1 is a schematic diagram showing an example of a gas-phase polymerization reactor 100 belonging to the horizontal polymerization reactor for producing a propylene polymer of the present invention. Fig. 2 is a schematic diagram showing an example of a horizontal polymerization reactor 200 in which a gas-phase polymerization process of a comparative example was carried out. Fig. 3 shows operational data showing the results of actual machine tests in which the horizontal polymerization reactor for producing a propylene polymer of the present invention and the horizontal polymerization reactor of the comparative example were operated for a long period of time.
[0020] The features of the horizontal polymerization reactor for producing a propylene polymer of the present invention (hereinafter, sometimes referred to as the "polymerization reactor of the present invention") will be specifically described in detail below. The explanation of the constituent elements described below is one example of an embodiment of the present invention, and the present invention is not limited to the following description as long as it does not deviate from the gist of the invention. In the present invention, the term "to" indicating a range of numerical values is used to mean that the numerical values before and after it are included as the lower limit and upper limit, respectively.
[0021] The polymerization reactor of the present invention is a horizontal polymerization reactor for producing a propylene-based polymer, comprising: a cylindrical reactor body having an internal space and including a polymerization reaction chamber and a bearing chamber separated by a partition wall that crosses the longitudinal direction of the internal space; an agitator having an agitator shaft that rotates in the circumferential direction of the reactor body and an agitator part fixed on the agitator shaft; a bearing that is disposed on at least one end side of the agitator shaft and receives an end of the agitator shaft; a pressure equalizing line connecting the polymerization reaction chamber and the bearing chamber; a purge gas supply line connected to at least the pressure equalizing line; and a catalyst supply nozzle that is connected to a catalyst supply port of the polymerization reaction chamber; wherein the agitator shaft penetrates the partition wall and is housed in the polymerization reaction chamber and the bearing chamber, the agitator part is housed in the polymerization reaction chamber, and the bearing is housed in the bearing chamber; The distance in the longitudinal direction of the polymerization reactor from a connection position between the catalyst supply port of the polymerization reaction chamber and the catalyst supply nozzle to a connection position between the polymerization reaction chamber and the pressure equalization line is 10% or more of the length of the polymerization reaction chamber.
[0022] The polymerization reactor of the present invention is a horizontal polymerization reactor for producing a propylene polymer by a gas-phase polymerization method. The propylene polymer produced using the polymerization reactor of the present invention includes a propylene homopolymer and a propylene copolymer. The polymerization reactor of the present invention is typically used to produce a propylene polymer in which the proportion of propylene-derived repeating units in the entire propylene polymer is 50 mol% or more in terms of the molar ratio of the repeating units or 50 mass% or more in terms of the mass ratio of the repeating units. The comonomer copolymerized with propylene as the main monomer is not particularly limited, but an α-olefin monomer other than propylene is preferably used from among α-olefin monomers having from 2 to 20 carbon atoms. Specific examples of the α-olefin monomer having 2 to 20 carbon atoms include ethylene, 1-butene, 3-methyl-1-butene, 4-methyl-1-pentene, 3-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 1-nonene, 1-octene, 1-heptene, 1-hexene, 1-decene, 1-undecene, and 1-dodecene.
[0023] Gas-phase polymerization is a polymerization process in which polymerization is carried out in a gas phase substantially in the absence of a liquid phase. It is sufficient that the phase in which polymerization is carried out is substantially a gas phase, and a liquid may be present within the scope of the present invention. Examples of this liquid include a liquefied monomer-containing liquid for heat removal and an inert hydrocarbon such as hexane used as a solvent when supplying a catalyst. A liquid-phase reaction in which a catalyst diluted in a solvent is supplied and then reacts with a liquefied monomer dissolved in the solvent is also included in the gas-phase polymerization of the present invention.
[0024] A horizontal polymerization reactor is a polymerization reactor in which a cylindrical reaction vessel is arranged in a direction such that, when the reactor is installed, the central axis extending in the longitudinal direction of the reaction vessel (longitudinal central axis) is approximately horizontal (i.e., a direction that can be considered to be perpendicular to the direction of gravity in the technical field of the present invention). The polymerization reactor of the present invention may be applied to continuous polymerization in which raw material monomers are continuously supplied into the reaction vessel and the produced polymer is withdrawn as the polymerization reaction progresses. When multistage polymerization is performed using the polymerization reactor of the present invention, two or more polymerization reactors of the present invention may be connected to perform multistage polymerization, or the polymerization reactor of the present invention may be connected to a polymerization reactor other than the present invention.
[0025] In the polymerization reactor of the present invention, the reaction vessel, which is a cylindrical reactor body, is divided into a polymerization reaction chamber and a bearing chamber by a partition wall that crosses the longitudinal direction of the internal space. The polymerization reaction chamber is a main chamber where the polymerization reaction takes place, and the bearing chamber is a small chamber that houses bearings. The internal space of the reaction vessel may be provided with a partition wall that separates the bearing chamber at one longitudinal end, and a second partition wall may be provided at the other longitudinal end.
[0026] The agitator has a stirring shaft that rotates in the circumferential direction of the barrel of the reactor body and a stirring unit fixed on the stirring shaft. The stirring unit is a member that applies a stirring force to the reaction materials in the reaction chamber and is also called a stirring blade. The shape of the stirring unit is not particularly limited, and it may be, for example, blade-shaped, screw-shaped, etc. Other settings of the stirring unit, such as dimensions (length, width, thickness), position on the stirring shaft, azimuth angle around the stirring shaft, and inclination angle with respect to the rotation direction, are also not particularly limited, and can be set appropriately taking into consideration the stirring force, material transport force in the flow direction, etc. The agitator is arranged so that the stirring shaft penetrates the partition wall and extends from the polymerization reaction chamber to the bearing compartment, and the stirring unit is accommodated in the polymerization reaction chamber. The agitator is usually arranged so that the longitudinal center axis of the internal space of the reactor body and the stirring shaft of the agitator overlap.
[0027] When the agitator is disposed in the reactor body, one end of the agitator shaft penetrates the partition wall and reaches the bearing compartment, where it is supported rotatably by a bearing disposed there. If necessary, bearings may be disposed in two or more locations, including a location other than the bearing compartment, and the agitator shaft may be supported by these multiple bearings. The agitator shaft is connected to a driving device such as a motor. By rotating the agitator part of the agitator in the polymerization reaction chamber, the starting materials and reaction products can be stirred, allowing efficient and uniform polymerization.
[0028] The reactor body of the polymerization reactor is provided with a supply port for supplying starting materials such as a catalyst, a cocatalyst, a main monomer, a comonomer, an inert solvent, and a molecular weight modifier into the polymerization reaction chamber, and a discharge port for withdrawing the reaction product. The reactor body is also provided with an inlet / outlet such as a recovery port for recovering unreacted monomer or unreacted gas, as needed, sensors such as a thermometer and a pressure gauge for monitoring the state of the reactor body, and other equipment.
[0029] In the present invention, the polymerization reaction chamber and the bearing compartment of the reactor main body are connected via a pressure equalization line that serves as a gas flow passage. The provision of the pressure equalization line reduces the pressure difference between the polymerization reaction chamber and the bearing compartment during long-term operation of the polymerization reactor, preventing damage to the partition wall. Furthermore, a purge gas supply line is connected to the pressure equalization line for gas purging. Purging the pressure equalization line with gas prevents fine powder of the propylene polymer produced in the polymerization reaction chamber from entering the pressure equalization line and further prevents the fine powder from passing through the pressure equalization line and entering the bearing compartment. The purge gas supply line is preferably connected to the pressure equalization line as well as the bearing. Purging the bearing with gas also prevents fine powder from entering the bearing compartment, even if it does enter the bearing compartment, from entering the sliding interface between the stirring shaft and the inner surface of the bearing. As the purge gas, an inert gas such as nitrogen or a raw material monomer / comonomer gas such as propylene or ethylene may generally be used, and propylene is particularly preferred when the purge gas is ultimately fed to the reaction chamber through a pressure equalization line as in the present invention. When a condensable gas such as propylene is used, the pressure equalization line or purge gas supply line may be wrapped with tracing or a heat-insulating material.
[0030] The pressure equalizing line is positioned so that the longitudinal distance of the polymerization reactor from the connection position between the catalyst supply port of the polymerization reaction chamber and the catalyst supply nozzle (i.e., the position of the catalyst supply port) to the connection position between the polymerization reaction chamber and the pressure equalizing line is 10% or more of the length of the polymerization reaction chamber. The longitudinal distance of the polymerization reactor from the connection position between the catalyst supply port of the polymerization reaction chamber and the catalyst supply nozzle to the connection position between the polymerization reaction chamber and the pressure equalizing line is preferably 14% or more, more preferably 20% or more. Since propylene polymer fine powder is distributed at a high density in a region of the internal space of the polymerization reaction chamber close to the connection position between the catalyst supply port of the polymerization reaction chamber and the catalyst supply nozzle, by positioning the connection position between the polymerization reaction chamber and the pressure equalizing line far away from the connection position between the catalyst supply port of the polymerization reaction chamber and the catalyst supply nozzle, the intrusion of fine powder from the polymerization reaction chamber into the pressure equalizing line can be reduced.
[0031] The catalyst supply nozzle is a nozzle connected to the catalyst supply port in order to inject the catalyst from the catalyst supply port into the polymerization reaction chamber. The polymerization reaction chamber and the catalyst supply line are connected via the catalyst supply nozzle. In the present invention, the catalyst supply nozzle may be a nozzle connected to the catalyst supply port not only for injecting the catalyst but also for injecting other catalyst components such as a cocatalyst. However, a nozzle connected to the supply port only for injecting catalyst components other than the catalyst without the intention of injecting the catalyst is not the catalyst supply nozzle of the present invention. In the present invention, the catalyst means solid particles having active sites capable of promoting the polymerization of propylene, and is to be distinguished from other catalyst components such as a cocatalyst.
[0032] The longitudinal distance of the polymerization reactor from the connection point between the catalyst supply port of the polymerization reaction chamber and the catalyst supply nozzle to the connection point between the polymerization reaction chamber and the pressure equalizing line refers to the length of a straight line connecting the center of the nozzle inner diameter at the connection point between the catalyst supply port of the polymerization reaction chamber and the catalyst supply nozzle to the center of the opening at the connection point between the polymerization reaction chamber and the pressure equalizing line. Furthermore, the length of the polymerization reaction chamber refers to the length of a straight line connecting the intersection point between the inner surface of the upstream end of the polymerization reaction chamber (i.e., the wall surface of the partition separating the polymerization reaction chamber from the bearing chamber facing the polymerization reaction chamber) and the longitudinal center axis of the polymerization reaction chamber, and the intersection point between the inner surface of the downstream end of the polymerization reaction chamber and the longitudinal center axis of the polymerization reaction chamber. When there are multiple connection positions between the catalyst supply port of the polymerization reaction chamber and the catalyst supply nozzle, or when there are multiple connection positions between the polymerization reaction chamber and the pressure equalizing line, the pressure equalizing line is arranged so that, among any combinations of the connection positions between the catalyst supply port of the polymerization reaction chamber and the catalyst supply nozzle and the connection positions between the polymerization reaction chamber and the pressure equalizing line, the combination with the shortest distance in the longitudinal direction of the polymerization reactor is 10% or more of the length of the polymerization reaction chamber.
[0033] The cross-sectional area of the pressure equalizing line is preferably such that the cross-sectional area (IA1) at the connection between the pressure equalizing line and the polymerization reaction chamber and the cross-sectional area (IA2) at the connection between the pressure equalizing line and the purge gas supply line satisfy the relationship expressed by the following formula: IA1<IA2. When the cross-sectional area (IA1) is smaller than the cross-sectional area (IA2), the flow rate of the purge gas in the direction toward the polymerization reaction chamber at the connection between the pressure equalizing line and the polymerization reaction chamber (FR1) and the flow rate (FR2) at the connection between the pressure equalizing line and the purge gas supply line satisfy the relationship expressed by the following formula: FR1>FR2. This allows the purge gas to be discharged from the pressure equalizing line into the polymerization reaction chamber at high speed, thereby preventing fine particles from entering the polymerization reaction chamber into the pressure equalizing line. By setting the flow velocity (FR1) of the purge gas toward the polymerization reaction chamber at the connection between the pressure equalization line and the polymerization reaction chamber, i.e., the discharge velocity of the purge gas from the pressure equalization line into the polymerization reaction chamber, to 0.2 m / sec or more, it is possible to stably prevent the intrusion of fine powder from the polymerization reaction chamber into the pressure equalization line.
[0034] Fig. 1 is a diagram showing an example of the configuration of a polymerization reactor (reactor 100) of the present invention, and a reactor vessel 1, which is the reactor body, is expressed as a cross-sectional schematic diagram. In Fig. 1, the reactor vessel 1 is a hollow vessel having an overall elongated shape consisting of a cylindrical body and hemispherical vessel ends connected to both ends of the body, and is arranged horizontally when the reactor 100 is installed.
[0035] The internal space of the reaction vessel 1 is provided with a partition wall 1a extending across the longitudinal direction at a position that is the boundary between the body portion at one end of the vessel and the hemispherical vessel end, and the partition wall 1a divides the internal space into a polymerization reaction chamber 1c and a bearing chamber 1b. The polymerization reaction takes place in the internal space of the polymerization reaction chamber 1c. In the case of the reactor 100, the partition wall 1a is the upstream end of the reaction, and the reaction space is surrounded by the inner surface of the body of the reaction vessel, the inner surface of the upstream partition wall 1a, and the inner surface of the downstream hemispherical end.
[0036] The internal space of the reaction vessel 1, including the polymerization reaction chamber 1c and the bearing compartment 1b, contains an agitator 2 having at least an agitator shaft 2a that rotates circumferentially around the body of the reaction vessel 1 and an agitator blade 2b fixed on the agitator shaft. The agitator 2 is arranged so that the longitudinal center axis of the reaction vessel coincides with the agitator shaft 2a, the agitator shaft 2a penetrates the partition wall 1a and is housed from the polymerization reaction chamber 1c to the bearing compartment 1b, and the agitator blade 2b is housed in the polymerization reaction chamber 1c. A bearing 3 is housed in the bearing compartment 1b provided at one end of the reaction vessel 1. A motor 4 is disposed at the other end of the reaction vessel 1 as a drive device for rotating the agitator shaft about its axis. One end of the agitator shaft 2a reaches the bearing compartment 1b and is inserted into the bearing 3, thereby being supported for rotation about its axis, and the other end of the agitator shaft 2a penetrates the outer wall of the reaction vessel 1 and is connected to the motor 4.
[0037] A co-catalyst supply port (position indicated by symbol D in FIG. 1 ) and a catalyst supply port (position indicated by symbol A in FIG. 1 ) are provided in this order from upstream to upstream in the upper portion of polymerization reaction chamber 1c in the direction of gravity and near the upstream end of the reaction chamber. A catalyst supply nozzle (not shown) is connected to the catalyst supply port, and polymerization reaction chamber 1c is connected to a catalyst supply line 8 via the catalyst supply nozzle. A co-catalyst supply nozzle (not shown) is connected to the co-catalyst supply port, and polymerization reaction chamber 1c is connected to a co-catalyst supply line 7 via the co-catalyst supply nozzle. Instead of providing separate and independent catalyst supply ports, only one catalyst component supply port for supplying the catalyst and co-catalyst may be provided, and a catalyst supply nozzle for supplying catalyst components such as the catalyst and co-catalyst may be attached to the supply port.
[0038] Furthermore, a plurality of raw material monomer supply ports and a plurality of unreacted gas vent ports are provided at appropriate intervals in the upper portion of the polymerization reaction chamber 1c in the direction of gravity and downstream of the catalyst supply port. Each raw material monomer supply port is connected to a raw material monomer supply line 9, and each unreacted gas vent port is connected to an unreacted gas vent line 10. Meanwhile, a plurality of raw material monomer gas supply ports are provided at appropriate intervals in the lower portion of the polymerization reaction chamber 1c in the direction of gravity, in regions facing the raw material monomer supply ports and the unreacted gas vent ports, provided within the reaction vessel 1. Each raw material monomer gas supply port is connected to a raw material monomer gas supply line 15. Furthermore, a polymer vent port is provided in the lower portion of the polymerization reaction chamber 1c in the direction of gravity and near the downstream end of the reaction, and a polymer vent line 19 is connected to it.
[0039] The polymerization reaction chamber 1c and the bearing chamber 1b of the reaction vessel 1 are each provided with an equalizing line connection port, and a pressure equalizing line 5 is connected to these two connection ports, thereby connecting the polymerization reaction chamber 1c and the bearing chamber 1b in a gas-flowable manner. A purge gas supply line 6 is connected to the equalizing line 5 and the bearing 3, and purge gas is supplied from the purge gas supply line to the equalizing line and the bearing. The purge gas to the equalizing line 5 is supplied to the polymerization reaction chamber 1c through the equalizing line. Meanwhile, the purge gas to the bearing 3 is supplied to the polymerization reaction chamber 1c through a small gap between the bearing 3 and the agitator shaft 2a. The equalizing line 5 is positioned so that the longitudinal distance of the polymerization reactor from the connection position between the catalyst supply port of the polymerization reaction chamber 1c and the catalyst supply nozzle (position indicated by symbol A in Figure 1) to the connection position between the polymerization reaction chamber 1c and the equalizing line 5 (position indicated by symbol B in Figure 1) is 10% or more of the length of the polymerization reaction chamber.
[0040] The method for producing a propylene polymer by gas phase polymerization using the reactor 100 will be described below.
[0041] The catalyst is introduced into the polymerization reaction chamber 1c through a catalyst supply port connected to a catalyst supply nozzle, and the cocatalyst is introduced through a cocatalyst supply port connected to a cocatalyst supply nozzle. The catalyst is not particularly limited as long as it can be used for the polymerization of olefin-based monomers, and for example, a Ziegler catalyst or a metallocene catalyst can be used. Other components, such as a cocatalyst such as an organoaluminum compound, may be supplied through the cocatalyst supply port, or may be supplied through the catalyst supply port as a component of the catalyst after contacting it with a Ziegler-based solid catalyst component or a metallocene complex component. The catalyst may be supplied to the reaction vessel as is in powder form, or may be supplied after diluting it with an inert solvent such as a liquid saturated hydrocarbon or mineral oil.
[0042] The raw materials, liquefied propylene and liquefied comonomer, are introduced into the polymerization reaction chamber 1c through a plurality of raw material monomer supply ports connected to a raw material monomer supply line 9. Gaseous raw materials (comonomer, hydrogen, etc.) are introduced into the polymerization reaction chamber 1c through a plurality of raw material monomer gas supply ports connected to a raw material monomer gas supply line 15. The propylene and comonomer introduced into the polymerization reaction chamber 1c are polymerized in a gas phase in contact with the catalyst while being stirred together with the reaction product by a stirrer, and a propylene-based polymer is synthesized. Hydrogen acts as a molecular weight regulator.
[0043] The polymerization conditions, such as temperature and pressure, of the gas-phase polymerization method are not particularly limited and can be set arbitrarily according to the raw material monomer. When the raw material monomer is propylene, the reaction temperature, polymerization pressure, and residence time in the reaction vessel are as follows. The lower limit of the reaction temperature is preferably 0°C or higher, more preferably 30°C or higher, and particularly preferably 40°C or higher, and the upper limit is preferably 100°C or lower, more preferably 90°C or lower, and particularly preferably 80°C or lower. The lower limit of the polymerization pressure is atmospheric pressure or higher, preferably 600 kPaG or higher, more preferably 1000 kPaG or higher, and particularly preferably 1600 kPaG or higher, and the upper limit is preferably 4200 kPaG or lower, more preferably 3500 kPaG or lower, and particularly preferably 3000 kPaG or lower. The residence time in the reaction vessel is arbitrarily adjusted according to the configuration of the reactor and the product index, but is generally set within the range of 30 minutes to 10 hours. The stirring speed of the stirrer is adjusted arbitrarily according to the reactor configuration, size, product index, etc., but generally, the number of rotations is 10 to 50 min -1 It is set within the range.
[0044] In the reaction vessel 1, the flow path cross-sectional area (IA1) of the pressure equalizing line 5 at the connection portion between the pressure equalizing line 5 and the polymerization reaction chamber 1c (the position indicated by symbol B in FIG. 1 ) and the flow path cross-sectional area (IA2) of the pressure equalizing line 5 at the connection portion between the pressure equalizing line 5 and the purge gas supply line 6 (the position indicated by symbol C in FIG. 1 ) have a relationship represented by the following formula: IA1<IA2. By making the flow path cross-sectional area (IA1) smaller than the flow path cross-sectional area (IA2), the flow rate (FR1) of the purge gas in the direction toward the polymerization reaction chamber at the connection between the pressure equalizing line and the polymerization reaction chamber (position indicated by symbol B in FIG. 1 ) and the flow rate (FR2) of the purge gas in the direction toward the polymerization reaction chamber at the connection between the pressure equalizing line and the purge gas supply line (position indicated by symbol C in FIG. 1 ) are related by the following formula: FR1 > FR2, and the purge gas can be discharged from the pressure equalizing line into the polymerization reaction chamber at high speed, thereby preventing the intrusion of fine particles from the polymerization reaction chamber into the pressure equalizing line. It is particularly preferable that the flow rate of the purge gas at the connection between the pressure equalizing line and the polymerization reaction chamber (position indicated by symbol B in FIG. 1 ) be 0.2 m / s or more in the direction from the connection between the pressure equalizing line and the purge gas supply line (position indicated by symbol C in FIG. 1 ) to the connection between the pressure equalizing line and the polymerization reaction chamber.
[0045] The heat of polymerization generated during polymerization is removed by the heat of vaporization (latent heat of vaporization) of the raw material liquefied propylene supplied through a raw material monomer supply line 9 located at the upper part of the polymerization reaction chamber 1c in the direction of gravity. Unreacted propylene gas is discharged to the outside of the reaction system through an unreacted gas vent line 10 located at the upper part of the polymerization reaction chamber 1c in the direction of gravity, passes through a bag filter 11, and is partially condensed in a condenser 12. The gas is separated into a liquid phase and a gas phase in a gas-liquid separation tank 16. To remove the heat of polymerization, the separated liquid phase is reintroduced via the raw material monomer supply line 9 by the driving force of a pump 13 into multiple raw material monomer supply ports located at the upper part of the polymerization reaction chamber 1c in the direction of gravity. Meanwhile, the separated gas phase is mixed with a comonomer gas, hydrogen for molecular weight control, and the like, and reintroduced via the raw material monomer gas supply line 15 by the driving force of a compressor 14 into multiple raw material monomer gas supply ports located at the lower part of the polymerization reaction chamber 1c in the direction of gravity. Propylene, the raw material, is supplied to gas-liquid separation tank 16 via raw material propylene etc. supply line 17. Other raw materials (comonomer, hydrogen, etc.) are supplied to the reaction system in the form of gas via gas raw material supply line 18, or in the form of liquid via raw material propylene etc. supply line 17. Polymer particles, the reaction product, move from the upstream to the downstream within the polymerization reaction chamber while being mixed by stirring, are discharged outside the reaction system via polymer withdrawal line 19, are separated in gas recovery machine 20, and are then recovered in powder recovery machine 21.
[0046] The present disclosure will be described in more detail below using examples, but the present invention is not limited to these examples. In these examples, propylene polymerization was carried out continuously over a long period of time using a horizontal polymerization reactor for producing a propylene-based polymer by gas phase polymerization. The polymerization reaction chamber and the bearing compartment of the polymerization reactor were connected via a pressure equalization line, and a purge gas supply line was connected to the pressure equalization line and the bearing. The pressure equalization line and the bearing were purged with gas during the polymerization reaction. During long-term operation of the polymerization reactor, the change over time in the differential pressure between the polymerization reaction chamber and the bearing compartment was observed.
[0047] 1. Example 1 Using a propylene polymerization reactor having the following configuration as shown in Figure 1, continuous polymerization was carried out over a long period of time under the following polymerization conditions. (1) Configuration of the polymerization reactor A horizontal gas-phase polymerization reactor was used, which had a polymerization reaction chamber length of 16 m, a vessel body with an inner diameter of the body of the polymerization reaction chamber of 2.9 m, and an agitator with an agitation shaft equipped with an agitation blade. The agitation shaft rotation speed was 16 min -1 (2) Configuration and arrangement of the pressure equalization line The longitudinal distance of the polymerization reactor from the connection position between the polymerization reaction chamber and the catalyst supply nozzle to the connection position between the polymerization reaction chamber and the pressure equalization line was 5.7 m, which was a distance equivalent to 35% of the length of the polymerization reaction chamber. The flow path cross-sectional area (IA1) of the pressure equalization line at the connection between the pressure equalization line and the polymerization reaction chamber was 4.9 cm 2 The cross-sectional area (IA2) of the pressure equalizing line at the connection between the pressure equalizing line and the purge gas supply line is 11.6 cm 2 The relationship was expressed by the following formula: IA1<IA2. (3) Flow rate of purge gas in pressure equalizing line The flow rate of purge gas in the direction toward the polymerization reaction chamber at the junction between the pressure equalizing line and the polymerization reaction chamber (FR1) was 0.28 m / sec, and the flow rate of purge gas in the direction toward the polymerization reaction chamber at the junction between the pressure equalizing line and the purge gas supply line (FR2) was 0.13 m / sec. (4) Polymerization conditions Polymerization temperature: 60 to 70°C Polymerization pressure: 2.2 to 2.5 MPaG Propylene homo-gas phase polymerization and propylene-ethylene random gas phase polymerization (5) Accumulated operating time Accumulated operating time: about 9 months
[0048] (6) Test Results The test results are shown by the solid line (Improved process) in the graph of Figure 3. The graph in Figure 3 shows the change in the differential pressure between the polymerization reaction chamber and the bearing chamber over time, with the horizontal axis representing the cumulative operating time and the vertical axis representing the ratio (Pressure difference / %) of the differential pressure between the polymerization reaction chamber and the bearing chamber when the internal pressure of the polymerization reaction chamber is taken as 100%. The ratio of the differential pressure between the polymerization reaction chamber and the bearing chamber when the internal pressure of the polymerization reaction chamber is taken as 100% was approximately 0.6% at the start of long-term operation, and this low differential pressure was maintained even after approximately 9 months of cumulative operating time had elapsed. The differential pressure remained stable during long-term operation, and no temporary fluctuations in the differential pressure were observed.
[0049] 2. Comparative Example 1 Using a propylene polymerization reactor having the following configuration as shown in Figure 2, continuous polymerization was carried out over a long period of time under the following polymerization conditions. (1) Configuration of the polymerization reactor A horizontal gas-phase polymerization reactor was used, which had a vessel body with a polymerization reaction chamber length of 16 m and a barrel inner diameter of 2.9 m, and was equipped with a stirrer having a stirring shaft fitted with a stirring blade. The stirring shaft rotation speed was 16 min -1 (2) Configuration and arrangement of the pressure equalization line The longitudinal distance of the polymerization reactor from the connection position between the polymerization reaction chamber and the catalyst supply nozzle to the connection position between the polymerization reaction chamber and the pressure equalization line was 0.62 m, which was a distance equivalent to 3.8% of the length of the polymerization reaction chamber. The flow path cross-sectional area (IA1) of the pressure equalization line at the connection between the polymerization reaction chamber and the pressure equalization line was 11.6 cm 2 The cross-sectional area (IA2) of the pressure equalizing line at the connection between the pressure equalizing line and the purge gas supply line is also 11.6 cm 2 (3) Flow rate of purge gas in pressure equalization line The flow rate of purge gas in the direction toward the polymerization reaction chamber at the junction between the pressure equalization line and the polymerization reaction chamber (FR1) was 0.13 m / sec, and the flow rate of purge gas in the direction toward the polymerization reaction chamber at the junction between the pressure equalization line and the purge gas supply line (FR2) was also 0.13 m / sec. (4) Polymerization conditions Polymerization temperature: 60 to 70°C Polymerization pressure: 2.2 to 2.5 MPaG Propylene homo-gas phase polymerization and propylene-ethylene random gas phase polymerization (5) Accumulated operating time Accumulated operating time: about 9 months
[0050] (6) Test Results The test results are shown by the dotted line ("Not improved process") in the graph in Figure 3. The graph in Figure 3 shows the change in the pressure difference between the polymerization reaction chamber and the bearing chamber over time, with the horizontal axis representing cumulative operating time and the vertical axis representing the pressure difference between the polymerization reaction chamber and the bearing chamber when the internal pressure of the polymerization reaction chamber is taken as 100% (Pressure difference / %). The pressure difference between the polymerization reaction chamber and the bearing chamber when the internal pressure of the polymerization reaction chamber is taken as 100% was approximately 0.6% at the start of long-term operation. However, after approximately three months of cumulative operating time, the pressure difference gradually increased, reaching approximately 1.1% after approximately six months and approximately 2.5% after approximately nine months. After approximately six months, the pressure difference became unstable, and sudden, temporary fluctuations in the pressure difference were frequently observed.
[0051] [Discussion of Examples] In the polymerization reactor of Comparative Example 1, the longitudinal distance of the polymerization reactor from the connection position between the polymerization reaction chamber and the catalyst supply nozzle to the connection position between the polymerization reaction chamber and the pressure equalization line was set to a distance equivalent to 3.8% of the length of the polymerization reaction chamber. In this polymerization reactor, the differential pressure between the polymerization reaction chamber and the bearing compartment gradually increased during long-term operation, and the differential pressure became unstable as the cumulative operating time increased. From this observation result, it is believed that in the polymerization reactor of Comparative Example 1, fine propylene polymer powder accumulated in the pressure equalization line during long-term operation, causing blockage of the pressure equalization line.
[0052] In the polymerization reactor of Example 1, the longitudinal distance from the connection point between the polymerization reaction chamber and the catalyst feed nozzle to the connection point between the polymerization reaction chamber and the pressure equalization line was set to a distance equivalent to 35% of the length of the polymerization reaction chamber. In this polymerization reactor, the differential pressure between the polymerization reaction chamber and the bearing compartment did not change during long-term operation, was maintained at the low differential pressure at the start of operation, and remained stable even with increasing cumulative operating time. From this observation result, it is believed that in the polymerization reactor of Example 1, propylene polymer fine powder did not accumulate in the pressure equalization line during long-term operation, and therefore no clogging of the pressure equalization line occurred.
[0053] DESCRIPTION OF SYMBOLS 100 Polymerization reactor 1 Reaction vessel 1a Partition wall 1b Bearing compartment 1c Polymerization reaction chamber 2 Agitator 2a Agitation shaft 2b Agitation blade 3 Bearing 4 Motor 5 Pressure equalization line 6 Purge gas supply line 7 Cocatalyst supply line 8 Catalyst supply line 9 Raw material monomer supply line 10 Unreacted gas withdrawal line 11 Bag filter 12 Condenser 13 Pump 14 Compressor 15 Raw material monomer gas supply line 16 Gas-liquid separation tank 17 Raw material propylene etc. supply line 18 Gaseous raw material supply line (comonomer, hydrogen etc.) 19 Polymer withdrawal line 20 Gas recovery machine 21 Powder recovery machine
Claims
1. A horizontal polymerization reactor for producing a propylene-based polymer, comprising: a cylindrical reactor body having an internal space and a polymerization reaction chamber and a bearing chamber separated by a partition wall that crosses the longitudinal direction of the internal space; an agitator having an agitator shaft that rotates in the circumferential direction of the reactor body and an agitator part fixed on the agitator shaft; a bearing that is disposed on at least one end side of the agitator shaft and receives an end of the agitator shaft; a pressure equalizing line connecting the polymerization reaction chamber and the bearing chamber; a purge gas supply line connected to at least the pressure equalizing line; and a catalyst supply nozzle connected to a catalyst supply port of the polymerization reaction chamber, wherein the agitator shaft penetrates the partition wall and is housed in the polymerization reaction chamber and the bearing chamber, the agitator part is housed in the polymerization reaction chamber, and the bearing is housed in the bearing chamber, a longitudinal distance of the polymerization reactor from a connection position between the catalyst supply port of the polymerization reaction chamber and the catalyst supply nozzle to a connection position between the polymerization reaction chamber and the pressure equalizing line is 10% or more of a length of the polymerization reaction chamber.
2. The horizontal polymerization reactor for producing a propylene polymer according to claim 1, wherein the flow path cross-sectional area of the pressure equalizing line is such that a flow path cross-sectional area (IA1) at a connection portion between the pressure equalizing line and the polymerization reaction chamber and a flow path cross-sectional area (IA2) at a connection portion between the pressure equalizing line and the purge gas supply line satisfy the following formula: IA1<IA2.
3. A method for producing a propylene polymer, comprising polymerizing a monomer containing propylene using the horizontal polymerization reactor for producing a propylene polymer according to claim 1 or 2.
4. A method for producing a propylene-based polymer according to claim 3, wherein a flow rate (FR1) of the purge gas in the direction toward the polymerization reaction chamber at a junction between the pressure equalization line and the polymerization reaction chamber and a flow rate (FR2) of the purge gas in the direction toward the polymerization reaction chamber at a junction between the pressure equalization line and the purge gas supply line have a relationship represented by the following formula: FR1>FR2.
5. The method for producing a propylene polymer according to claim 3 or 4, wherein the flow rate (FR1) of the purge gas in the direction toward the polymerization reaction chamber at the connecting portion between the pressure equalization line and the polymerization reaction chamber is 0.2 m / sec or more.
6. The method for producing a propylene-based polymer according to any one of claims 3 to 5, wherein a purge gas containing propylene is used.
Citation Information
Patent Citations
Polypropylene continuous production equipment for fine powder barrier production
CN110523349A
Horizontal reactor
JP1988223001A
Polymerization of α-olefins
JP1995504708A
Method for producing propylene-based polymer
JP2017095606A