Decoration member

The decorative member with a synthetic resin or glass base and metal-containing particles coated in a transparent organic layer addresses the issues of millimeter wave transmission loss and infrared transmittance, enhancing object detection and maintaining a metallic luster for vehicle applications.

WO2024202132A1PCT designated stage expired Publication Date: 2024-10-03IKUYO
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/035344
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2023-09-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional decorative coatings with metal nanoparticles suffer from high millimeter wave transmission loss and inadequate infrared transmittance, making it difficult to detect small objects and maintain a metallic luster, especially when used in conjunction with millimeter wave radar and lidar systems on vehicles.

Method used

A decorative member featuring a synthetic resin or glass base material with metal-containing particles, each coated with a transparent organic layer and a protective layer, ensuring low millimeter wave transmission loss and high infrared transmittance, while maintaining a metallic luster through controlled particle distribution and thickness.

Benefits of technology

The solution achieves reduced millimeter wave transmission loss (0.001-6 dB) and high infrared transmittance (80-94%), along with excellent metallic luster, enabling effective detection of objects and maintaining an aesthetic appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023035344_03102024_PF_FP_ABST
    Figure JP2023035344_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a decorative member having high infrared transmittance, low millimeter-wave transmission loss, and excellent metallic luster. The decorative member comprises: a substrate including a synthetic resin; a plurality of metal-containing particles disposed on the surface of the substrate, each having a metal particle and a translucent organic layer on the surface of the metal particle; and a protective coating layer that covers the plurality of metal-containing particles on the surface of the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

decorative materials

[0001] The present invention relates to a decorative member used, for example, in an exterior part of a vehicle.

[0002] In recent years, for the purpose of autonomous driving (automated travel), technologies have been considered that use a distance measuring sensor mounted on the front of a vehicle to measure the distance and relative speed between the vehicle and a preceding vehicle or obstacle, and control the distance between the vehicle and the preceding vehicle while accelerating or decelerating the vehicle based on this measurement information. Radio wave transmitting and receiving devices such as millimeter-wave radar and LiDAR (Light Detection and Ranging) are used as distance measuring sensors.

[0003] To maximize its performance, radio wave transmitters and receivers such as millimeter-wave radars are preferably installed in a central position in the front of the vehicle, and are often installed, for example, behind exterior components such as vehicle emblems or covers. In this case, the millimeter waves emitted from the radio wave transmitter and receiver are emitted forward through a decorative member or the like, and then reflected by a preceding vehicle or obstacle, and the reflected waves are received by the radio wave transmitter and receiver again through the decorative member. Therefore, it is desirable for the exterior components to be made of decorative members that have low millimeter-wave transmission loss and an excellent aesthetic appearance due to their metallic luster.

[0004] Known decorative coatings formed within the millimeter wave path of millimeter wave radar include those in which, for example, gold, silver, tin, indium, or other metal nanoparticles are dispersed in a binder layer (see, for example, Patent Document 1).

[0005] Millimeter-wave radar can have difficulty detecting small objects and obstacles with low reflectivity, such as cardboard. Because LIDAR uses infrared light with a shorter wavelength than millimeter-wave radar, it can generally detect smaller objects than millimeter-wave radar, and 3D LIDAR can be used to obtain a three-dimensional image of the surrounding environment.

[0006] JP 2013-185869 A

[0007] However, conventional decorative coatings in which metal nanoparticles are dispersed in a binder layer have the disadvantage that the metal nanoparticles cause diffuse reflection of light, making it difficult to achieve a sufficient metallic luster. Even if the decorative coating is formed within the infrared path of the lidar, it is difficult to achieve sufficient infrared transmission and reception and a metallic aesthetic.

[0008] The present invention has been made in consideration of the above-mentioned problems of the prior art, and has as its object to provide a decorative member that has high infrared transmittance, low millimeter wave transmission loss, and excellent metallic luster.

[0009] The decorative member of the present invention is characterized by comprising a substrate containing synthetic resin or glass, a plurality of metal-containing particles arranged on the surface of the substrate, each of which has a metal particle and a translucent organic layer on the surface of the metal particle, and a protective coating layer covering the plurality of metal-containing particles on the surface of the substrate.

[0010] In the decorative member, the area occupancy rate (herein also simply referred to as occupancy rate) of the plurality of metal-containing particles when the surface of the substrate is viewed from above is preferably 0.3 to 9%.

[0011] In the decorative member of the present invention, the occupancy rate of the plurality of metal-containing particles is 0.3 to 9%, and the metal particles among the metal-containing particles are hardly in contact with or overlap with each other. Therefore, infrared rays with wavelengths in the range of 905 to 1550 nm and millimeter waves with frequencies in the range of 70 to 100 GHz can pass through the gaps between adjacent metal-containing particles, or at least the gaps between the metal particles, thereby reducing transmission loss.

[0012] Furthermore, the metal-containing particles essentially consist of only metal particles and a light-transmitting organic layer provided on the surface of the metal particles, and the metal particles are held in place by the organic layer, ensuring flatness and increasing the amount of reflected light, so that excellent metallic luster can be obtained even when multiple metal-containing particles are arranged far apart.

[0013] The decorative member of the present invention has an attenuation factor, as an index of millimeter wave transmission loss, in the range of 0.001 to 6 dB, an infrared transmittance in the range of 80 to 94%, and an L* value (brightness), as an index of metallic gloss, measured from the substrate side, in the range of 20 to 80, preferably in the range of 20 to 60, and more preferably in the range of 20 to 40.

[0014] Furthermore, in the decorative member of the present invention, metallic luster cannot be obtained if the L* value (brightness) exceeds 80. Furthermore, it is technically difficult to make the L* value (brightness) less than 20.

[0015] In the decorative member of the present invention, if the attenuation rate exceeds 6 dB, the transmission loss of millimeter waves becomes large and millimeter waves cannot be substantially transmitted. Furthermore, it is technically difficult to achieve an attenuation rate of less than 0.001 dB.

[0016] In order to impart a beautiful appearance of metallic luster to the decorative member of the present invention, it is preferable that the plurality of metal-containing particles are scattered uniformly on the surface of the substrate when the surface of the substrate is viewed in a plane.

[0017] In order to impart a beautiful appearance with metallic luster to the decorative member of the present invention, it is preferable that the metal particles in the decorative member are in the form of flakes with a film thickness of 0.01 to 0.03 μm, and the organic layer has a film thickness of 0.5 to 1 μm and is provided on the front and back surfaces, or on either the front or back surface, of the metal particles.

[0018] In the decorative member, the metal particles of the plurality of metal-containing particles are preferably aluminum flake particles.

[0019] In the decorative member, the plurality of metal-containing particles are preferably present only within a thickness range of up to 5 μm from the surface of the substrate. If the decorative member of the present invention has a thickness exceeding 5 μm, the transmission loss of millimeter waves may become excessive.

[0020] In order to impart a beautiful metallic luster to the decorative member of the present invention, the plurality of metal-containing particles in the decorative member preferably have an average particle size in the range of 10 to 35 μm.

[0021] In the decorative member, the protective coating layer preferably has a thickness of 10 to 50 μm. Each of the plurality of metal-containing particles 4 essentially consists of metal particles and a translucent organic layer on the surface of the metal particles. If the surfaces of the metal particles are exposed to the atmosphere, for example, there is a risk that the individual metal-containing particles will peel off from the substrate surface. However, by providing the protective coating layer with a thickness of 10 to 50 μm, peeling of the metal-containing particles can be prevented. If the protective coating layer is less than 10 μm thick, the corners of the metal particles and the organic layer will not be sufficiently covered, and there is a risk of particle peeling. If it exceeds 50 μm, sagging will occur easily, which may impair the appearance.

[0022] In the decorative member, the substrate preferably includes a base and a primer layer on the surface of the base that forms the substrate surface. By providing the primer layer, the adhesion of the metal-containing particles to the substrate via the primer layer can be improved. Furthermore, by incorporating a black pigment or the like into the primer layer, the metallic luster of the metal-containing particles can be enhanced when the protective coating layer is on the visible side (surface coating system).

[0023] In the decorative member, a coating film is preferably formed on the surface of the substrate between adjacent ones of the plurality of metal-containing particles, which can improve the adhesion of the plurality of metal-containing particles to the substrate.

[0024] In the decorative member, the protective coating layer is preferably a light-transmitting layer made of a light-transmitting material, which allows the metal-containing particles to exhibit a beautiful appearance due to their metallic luster when the protective coating layer is on the visible side (surface coating system).

[0025] Furthermore, in the decorative member, when the substrate is on the viewer's side (backside coating system), the substrate may be a light-transmitting layer made of a light-transmitting material, and the protective coating layer may contain a black pigment or the like. In this case, the light-transmitting layer of the substrate can exhibit the aesthetic appearance of the metallic luster of the multiple metal-containing particles. Furthermore, in this case, the decorative member 1 in which the light-transmitting substrate is on the viewer's side may have a light-transmitting base layer made of a light-transmitting material between the light-transmitting substrate and the multiple metal-containing particles.

[0026] Therefore, the decorative member of the present invention comprises a substrate containing synthetic resin or glass, a plurality of metal-containing particles disposed on the surface of the substrate, each of the metal particles having a metal particle and a light-transmitting organic layer on the surface of the metal particle, and a protective coating layer covering the plurality of metal-containing particles on the surface of the substrate, wherein the plurality of metal-containing particles are uniformly scattered on the surface of the substrate when viewed from above, the occupancy of the plurality of metal-containing particles when viewed from above is 0.3 to 9%, the attenuation rate when millimeter waves having a frequency in the range of 60 to 90 GHz are transmitted is in the range of 0.001 to 6 dB, the transmittance when infrared rays having a wavelength in the range of 905 to 1550 nm are transmitted is 80 to 94%, and the L* value (brightness) measured from the substrate side is in the range of 20 to 80.

[0027] FIG. 1 is a partial cross-sectional view showing the configuration of a decorative member according to an embodiment of the present invention. FIG. 1 is a partial cross-sectional view showing the configuration of one metal-containing particle, of the plurality of metal-containing particles of the decorative member according to an embodiment of the present invention, having organic material layers on both sides of the metal particle. FIG. 1 is a partial cross-sectional view showing the configuration of one metal-containing particle, of the plurality of metal-containing particles of the decorative member according to an embodiment of the present invention, having an organic material layer on one side of the metal particle. FIG. 1 is a partial cross-sectional view showing a configuration of a modified decorative member according to an embodiment of the present invention, having no base layer. FIG. 1 is a partial cross-sectional view showing a configuration of a modified decorative member according to an embodiment of the present invention, having a coating film between adjacent metal-containing particles. FIG. 1 is a partial cross-sectional view showing a configuration of a modified decorative member according to an embodiment of the present invention, having a coating film between adjacent metal-containing particles but no base layer. FIG. 2 is a graph showing the relationship between the fine particle occupancy (Al occupancy) of a plurality of metal-containing particles in a decorative member according to an embodiment of the present invention and the infrared transmittance (wavelength 905 nm), based on the results of measuring the infrared transmittance of a decorative member according to an embodiment of the present invention. FIG. 2 is a graph showing the relationship between the fine particle occupancy (Al occupancy) of a plurality of metal-containing particles in a decorative member according to an embodiment of the present invention and the infrared transmittance (wavelength 1550 nm), based on the results of measuring the infrared transmittance of a decorative member according to an embodiment of the present invention. Photographs of a plurality of Al-containing particles (sample No. 2P) of a decorative member obtained in accordance with an example of the present invention. Photographs of a plurality of Al-containing particles (sample No. C3) of a decorative member obtained in accordance with an example of the present invention. Photographs of a plurality of Al-containing particles (sample No. C-2-1 / 2-2P) of a decorative member obtained in accordance with an example of the present invention. Photographs of a plurality of Al-containing particles (sample No. C-3-1) of a decorative member obtained in accordance with an example of the present invention. Photographs of a plurality of Al-containing particles (sample No. Metallic IS) of a decorative member obtained in accordance with an example of the present invention. Photographs of a plurality of Al-containing particles (sample No. Metallic M) of a decorative member obtained in accordance with an example of the present invention.

[0028] Next, embodiments of the present invention will be described in more detail with reference to the accompanying drawings.

[0029] The decorative member 1 of this embodiment is used, for example, as an exterior component that is provided on the path of infrared rays or millimeter waves transmitted and received by radio wave transmitting and receiving devices such as lidars and millimeter wave radars mounted on vehicles, etc.

[0030] As shown in Figure 1, the decorative member 1 includes, for example, a substrate 2 (base) made of synthetic resin with a base layer 2a on the substrate surface 2H, a plurality of metal-containing particles 4 arranged on the base layer 2a, and a guard coat 5 made of a translucent material as a protective coating layer that covers the plurality of metal-containing particles 4 on the substrate surface 2H.

[0031] As shown in FIGS. 2A and 2B, each of the plurality of metal-containing particles 4 has a metal particle 4a and a light-transmitting organic layer 4b provided on the surface thereof.

[0032] The metal particles 4a of the metal-containing particles 4 are flaky and have a film thickness of 0.01 to 0.03 μm. The organic material layer 4b of the metal-containing particles 4 has a film thickness of 0.5 to 1 μm. The organic material layer 4b of the metal-containing particles 4 is provided on both the front surface obv and the back surface rev of the metal particles 4a, as shown in FIG. 2A, or on one surface of the metal particles 4a, such as the front surface obv, as shown in FIG. 2B. The thickness of the multiple metal-containing particles 4 (metal particles 4a and organic material layer 4b) can be measured using an electron microscope or the like.

[0033] Examples of materials for the flaky metal particles 4a of the plurality of metal-containing particles 4 include metals such as tin, indium, aluminum, zinc, gold, titanium, and nickel, and alloys based on any of these metals. Examples of materials for the organic layer 4b include polyurethane resin, polymethyl methacrylate resin, epoxy resin, silicone resin, polycarbonate resin, and polyethylene terephthalate resin.

[0034] The metal-containing particles 4 are produced, for example, by the following process. First, a metal or alloy material for the metal particles 4a is vapor-deposited onto a film made of the material for the organic layer 4b to produce a metal-deposited film. Alternatively, an additional film made of the material for the organic layer 4b is laminated onto the metal particle 4a side of the metal-deposited film to produce an organic-metal-deposited film. Next, the metal-deposited film or the organic-metal-deposited film is pulverized to produce miscellaneous metal-containing particles, and the granulated metal-containing particles are then sized to produce a plurality of metal-containing particles having an average particle diameter of 10 to 35 μm. Aluminum flake-shaped particles are the metal particles 4a derived from vapor-deposited aluminum, which provide a desirable surface smoothness. Therefore, using aluminum flake-shaped particles is preferable for increasing the brightness of the decorative member 1 and achieving a high metallic texture. The plurality of metal-containing particles 4 preferably have an average particle diameter in the range of 10 to 35 μm.

[0035] As shown in Figure 3, in a modified example of the decorative member of the embodiment, the decorative member 1 can have a configuration without a base layer, for example, a base material 2 made of synthetic resin, a plurality of metal-containing particles 4 arranged on the base material surface 2H, and a guard coat 5 covering the plurality of metal-containing particles 4 on the base material surface 2H.

[0036] As shown in Figure 4, as a further modified configuration of the decorative member of the embodiment, the decorative member 1 can include, for example, a substrate 2 (base) made of synthetic resin with a primer layer 2a on the substrate surface 2H, a plurality of metal-containing particles 4 arranged on the primer layer 2a and a coating film 4C between adjacent ones of the plurality of metal-containing particles, and a guard coat 5 covering the plurality of metal-containing particles 4 on the substrate surface 2H.

[0037] As shown in Figure 5, as a modified example of the decorative member of the embodiment shown in Figure 4 without a base layer, the decorative member 1 can include, for example, a substrate 2 made of synthetic resin, a plurality of metal-containing particles 4 arranged on the substrate surface 2H and a coating film 4C between adjacent ones of the plurality of metal-containing particles, and a guard coat 5 covering the plurality of metal-containing particles 4 on the substrate surface 2H.

[0038] Examples of synthetic resins that may be used to form the substrate 2 include acrylic resin, polycarbonate resin, urethane (PUR) resin, AES (acrylonitrile ethylene styrene) resin, PET (ethylene terephthalate) resin, polyamide resin, epoxy resin, PBT (polybutylene terephthalate) resin, 66 nylon (PA) resin, and PF (phenol) resin.

[0039] The underlayer 2a is preferably one that has adhesive properties to the plurality of metal-containing particles 4 and the substrate 2, and examples thereof include paints whose main component is a synthetic resin, such as urethane paint, epoxy paint, ultraviolet-curable paint, and ambient-drying paint. Examples of such paints include a mixture of a main component (product name: R-241 MB-2.0 Primer), a curing agent (product name: R-255), and a thinner (product name: T-801) manufactured by Nippon Paint Automotive Coatings Co., Ltd., in a mass ratio of 100:7:70.

[0040] The underlayer 2 a may contain a coloring material with high infrared transmittance, such as black or red, etc. Examples of the coloring material include black pigments with an average particle size of about several hundred nanometers, such as carbon black, perylene black, or aniline black, and red pigments such as perylene red, and other pigments of various hues.

[0041] Furthermore, coloring can be applied anywhere on the substrate 2 or the metal-containing particles 4 in addition to the underlayer 2 a.

[0042] The plurality of metal-containing particles 4 can be formed by applying a metal-containing particle dispersion liquid, in which metal-containing particles are dispersed in a volatile solvent, onto the underlayer 2a and then evaporating the volatile solvent. The metal-containing particle dispersion liquid may be diluted with the volatile solvent as a diluent (thinner).

[0043] Examples of the volatile solvent include isopropanol, methanol, ethanol, toluene, xylene, ethyl acetate, butyl acetate, methyl ethyl ketone, and cyclohexanenone. Any one of the volatile solvents may be used alone, or two or more may be mixed and used. The volatile solvent in which the metal-containing particles 4 are dispersed and the volatile solvent used as a diluent may be the same or different.

[0044] An example of the metal-containing particle dispersion liquid is one containing butyl acetate as a dispersion medium and 0.4 mass % of metal-containing particles 4 having an average particle size of 10 to 35 μm. When forming a coating film 4C between the metal-containing particles 4, the metal-containing particle dispersion liquid may contain the same paint components as those of the underlayer 2a. In this way, after the plurality of metal-containing particles 4 are applied, the volatile solvent volatilizes to form the coating film 4C.

[0045] The metal-containing particles 4 are oriented so as to be approximately parallel to the surface of the substrate surface 2H. That is, the orientation angle of the metal-containing particles 4 relative to the surface of the substrate surface 2H (the angle formed with the substrate surface 2H) is several degrees or less. After a coating material containing the metal-containing particles 4 is applied to the substrate surface 2H or the underlayer 2a, the coating film shrinks in volume due to evaporation of the solvent during drying, making the coating film thinner. Utilizing this, the metal-containing particles 4 are arranged so that the orientation angle is several degrees or less (preferably 2 degrees or less). The height of the multiple metal-containing particles 4 from the underlayer 2a (or the substrate surface 2H if there is no underlayer) may be 5 μm or less. If the height of the metal-containing particles 4 exceeds 5 μm, the brilliance decreases.

[0046] The area occupancy rate (also referred to as "occupancy rate") is the percentage of the area occupied by the projected portion of the metal-containing particles 4 on the surface of the substrate surface 2H or the surface of the underlayer 2a when all of the metal-containing particles 4 after application of the plurality of metal-containing particles 4 are projected onto the surface.

[0047] When the plurality of metal-containing particles 4 applied to the substrate surface 2H or the underlayer 2a is observed in a plan view, the plurality of metal-containing particles 4 can be visually recognized. Therefore, the occupancy rate can be determined from an image obtained by photographing the plurality of metal-containing particles 4 through the guard coat 5 that covers the plurality of metal-containing particles 4.

[0048] The plurality of metal-containing particles 4 have an average particle diameter in the range of 10 to 35 μm, and the thickness of the plurality of metal-containing particles 4 is thin (for example, about 2 μm), so that the plurality of metal particles 4 a are substantially parallel to the substrate surface 2H (underlayer 2 a). In this state, if the plurality of metal-containing particles 4 occupy 0.3 to 9% when the substrate surface 2H is viewed in plan, and are uniformly distributed scattered on the substrate surface 2H (underlayer 2 a), a decorative member having high infrared transmittance, low millimeter wave transmission loss, and excellent metallic luster can be obtained.

[0049] The guard coat 5 can prevent individual metal-containing particles from peeling off and falling off from the plurality of metal-containing particles 4, and examples thereof include paints whose main component is a synthetic resin, such as two-component urethane paint, epoxy paint, ultraviolet-curable paint, and ambient-drying paint. Examples of such paints include those made by mixing a main component (product name: R-227), a curing agent (product name: R-255), and a thinner (product name: T-801), all manufactured by Nippon Paint Automotive Coatings Co., Ltd., in a mass ratio of 100:10:100.

[0050] The decorative member 1 of this embodiment, which is composed of a plurality of metal-containing particles 4, has an attenuation factor, which is an index of transmission loss when millimeter waves having a frequency in the range of 60 to 90 GHz pass through, in the range of 0.001 to 6 dB, a transmittance of infrared rays with wavelengths of 905 to 1550 nm (also referred to as IR transmittance) in the range of 80 to 94%, and an L* value (brightness), which is an index of metallic luster measured from the substrate 2 side, in the range of 20 to 80, preferably 28 to 60, and more preferably 28 to 40.

[0051] As such, the decorative member 1 of this embodiment is configured to include a base layer 2a located between the substrate 2 and the plurality of metal-containing particles 4, and a guard coat 5 as a light-transmitting layer located on the plurality of metal-containing particles 4, as shown in Figure 1.

[0052] The decorative member 1 of this embodiment is not limited to the configuration shown in Figure 1. Furthermore, the decorative member 1 of this embodiment may have a modified configuration in which the base layer 2a is omitted from the configuration shown in Figure 1, as shown in Figure 3, or a modified configuration in which a coating film 4C is provided between adjacent ones of the plurality of metal-containing particles in the configuration shown in Figure 1, as shown in Figure 4, or a modified configuration in which a coating film 4C is provided between adjacent ones of the plurality of metal-containing particles in the configuration shown in Figure 1 but the base layer 2a is omitted, as shown in Figure 5.

[0053] Example Embodiment In this example embodiment, the relationship between the occupancy rate of a plurality of metal-containing particles in a decorative member and IR transmittance (wavelengths of 905 nm and 1550 nm) was investigated.

[0054] First, various aluminum (Al)-containing particles (Al vapor deposition) with an average particle size of 10 to 35 μm were prepared as various metal-containing particles 4. Each Al-containing particle had 0.01 μm-thick metal particles 4a (thin flake-like vapor-deposited Al) sandwiched on both sides by 1 μm-thick silicone films (organic layers 4b). The prepared multiple Al-containing particles were sized to prepare Al-containing particles with an average particle size of 10 to 35 μm.

[0055] Next, an infrared-transmitting black paint was applied to the substrate 2 made of polycarbonate (PC) resin and dried at 80° C. for 30 minutes to form a 20 μm-thick underlayer 2 a.

[0056] Next, the metal-containing particle dispersion (a butyl acetate dispersion containing 0.4 mass % of the above-prepared Al-containing particles having an average particle size of 10 to 35) was applied to the underlayer 2a using a predetermined spray device so as to be uniformly distributed and scattered on the underlayer 2a, and then dried at room temperature for 10 minutes to form a plurality of metal-containing particles 4. In this case, a spray coater for the metal-containing particle dispersion was used to form a plurality of metal-containing particles 4 on a plurality of substrates 2 (referred to as "vapor-deposited Al organic material") such that the Al-containing particle occupancy (also referred to as Al occupancy) of the plurality of metal-containing particles 4 gradually increased from 0% (referred to as "PC material").

[0057] In addition, unlike the above-mentioned metal-containing particle dispersion liquid, an Al-containing particle dispersion liquid of butyl acetate in which multiple thin-film vapor-deposited Al metal particles 4a were dispersed at 5 mass% was applied onto the underlayer 2a, and multiple metal-containing particles 4 were formed in the same manner as in the case of the above-mentioned metal-containing particle dispersion liquid (referred to as "vapor-deposited Al only").

[0058] Next, a paint made by mixing a base agent (product name: R-227), a curing agent (product name: R-255), and a thinner (product name: T-801) manufactured by Nippon Paint Automotive Coatings Co., Ltd. in a mass ratio of 100:10:100 was applied onto each of the plurality of metal-containing particles 4, and the paint was dried at 80°C for 30 minutes to form a guard coat 5 with a thickness of 20 μm, thereby obtaining a plurality of decorative members 1.

[0059] Next, the IR transmittance (%) of the decorative member 1 obtained in this embodiment was measured when infrared (IR) rays with wavelengths of 905 nm and 1550 nm were transmitted through it.

[0060] The relationship between Al occupancy and IR transmittance (wavelengths 905 nm and 1550 nm) was measured using an infrared spectrophotometer (UV-3100PC) manufactured by Shimadzu Corporation, and Al occupancy was measured using a digital microscope (VHX-950F) manufactured by Keyence Corporation. The decorative member of this embodiment was positioned so that the guard coat faced the transmitting side of the device, and the relationship between Al occupancy and IR transmittance was measured. The results are shown in Table 1. Figures 6 and 7 are graphs based on the results in Table 1 showing the relationship between the fine particle occupancy (Al occupancy) of multiple metal-containing particles in the decorative member and IR transmittance (wavelengths 905 nm and 1550 nm). In Table 1 and Figures 6 and 7, Al occupancy (fine particle occupancy) of 0.9 to 8.08% corresponds to "vapor-deposited Al organic material," and Al occupancy (fine particle occupancy) of 9.85 to 40.69% corresponds to "vapor-deposited Al only."

[0061]

[0062] From Table 1 and Figures 6 and 7, it is clear that the decorative member 1 obtained in this embodiment, which comprises a plurality of metal-containing particles with an average particle diameter of 10 to 35 μm, each of which has metal particles (vapor-deposited Al organic material) and a translucent organic material layer on the surface of the metal particles, has an Al occupancy rate of 0.3 to 9% for the plurality of metal-containing particles, and has an IR transmittance of 80 to 94% when infrared rays with wavelengths in the range of 905 to 1550 nm pass through, and has an excellent metallic luster.

[0063] Next, various examples of decorative members were prepared in the same manner as in the above-described embodiment, each comprising a plurality of metal-containing particles each having metal particles (vapor-deposited Al organic material) and a translucent organic material layer on the surface of the metal particles. In these examples, aluminum (Al)-containing particles with an average particle size of 15 to 35 μm were prepared as various metal-containing particles. Each Al-containing particle comprised 0.01 μm-thick flaky vapor-deposited Al metal particles, sandwiched between two silicone films (organic material layers) with a thickness of 1 μm or 1.5 μm. By sizing the plurality of Al-containing particles, various types of metal-containing particles with an average particle size of 15 to 35 μm were prepared. Then, similar to the above-described embodiment, an Al-containing particle dispersion was prepared, and a plurality of Al-containing particles were formed on the undercoat layer of each substrate using a spray coater with the Al occupancy shown in Tables 2 to 8 below, to produce decorative members for Examples 1 to 24, respectively.

[0064] Examples 1 to 24: The attenuation factor, which is the transmission loss when millimeter waves are transmitted through the decorative members of Examples 1 to 4, the infrared transmittance (%) when infrared rays with wavelengths of 905 nm and 1550 nm are transmitted through the decorative members, and the L* value (brightness), which is an index of metallic luster, were measured. The infrared transmittance (%) when infrared rays with wavelengths of 905 nm and 1550 nm are transmitted through the decorative members of Examples 5 to 24, and the L* value (brightness), which is an index of metallic luster, were measured.

[0065] The attenuation rate was measured for millimeter waves in the frequency band of 60 to 90 GHz using a transmission attenuation rate measuring device (product name: Vector Network Analyzer N5227A) manufactured by Keycom Corporation, using a transmission attenuation measuring jig with a dielectric lens manufactured by Keycom Corporation, with the base side of the decorative member of this example placed facing the transmitting side of the device. The results are shown in Table 2 below.

[0066] The L* value (brightness) was measured from the side of the polycarbonate resin or glass guard coat 5 using a spectrophotometer (product name: CM-600d) manufactured by Konica Minolta, Inc., using a D65 light source and the SCI method including specular reflection light. The results are shown in Tables 2 to 8 below.

[0067] Comparative Examples 1 to 3: In the experiments, decorative members were produced in the same manner as in Example 1, except that the Al occupancy rate was set to 9.85 to 25.64%, the organic layer thickness was set to 0 to 2 μm, and the Al-containing particle diameter was set to 10 μm. The results of the comparative examples are shown in Table 9. However, when the organic layer thickness was less than 0.5 μm, the metallic appearance was reduced due to technical difficulties, and when the organic layer thickness was more than 1 μm, the metal-containing particles curled, resulting in poor appearance, so infrared transmittance was not measured.

[0068]

[0069]

[0070]

[0071]

[0072]

[0073]

[0074]

[0075] From the above Examples 1 to 24 and Comparative Examples 1 to 3, it was revealed that, in these decorative members, if the metal particles are in the form of flakes with a film thickness of 0.01 to 0.03 μm, the organic layer has a film thickness of 0.5 to 1 μm, and the occupancy rate of the plurality of metal-containing particles is 0.3 to 9%, the infrared transmittance exceeds 80%, the L* value (brightness) as an index of metallic gloss is small, a metallic feel (a glittering feel) is obtained, and the attenuation rate as an index of transmission loss when millimeter waves pass through is small.

[0076] Furthermore, similarly to the above-described embodiment, an Al-containing particle dispersion was prepared, and a plurality of Al-containing particles was formed on the undercoat layer of each substrate using a spray coater at the Al occupancy rate of the sample No. shown in Table 9 below, to produce each decorative member. The substrate surface was photographed through the guard coat covering the plurality of Al-containing particles, and photographed images of the plurality of Al-containing particles in the resulting decorative member are shown in Figures 8 to 13.

[0077]

[0078] From Table 9, it is clear that the decorative members of sample Nos. C3, C-2-1 / 2-2P, and C-3-1 can provide a metallic feel (a glittering feel).

[0079] 1 Decorative member 2H Base material surface 2 Base material (base) 2a Base layer 4 Metal-containing particles 4a Metal particles 4b Organic layer 4C Paint film 5 Guard coat (protective coating layer)

Claims

1. A decorative member comprising: a substrate containing synthetic resin or glass; a plurality of metal-containing particles arranged on a surface of the substrate, each of the metal particles having a metal particle and a light-transmitting organic layer on the surface of the metal particle; and a protective coating layer covering the plurality of metal-containing particles on the surface of the substrate.

2. A decorative member according to claim 1, characterized in that the occupancy rate of the plurality of metal-containing particles in a plan view of the surface of the base material is 0.3 to 9%.

3. A decorative member according to claim 1, characterized in that the metal particles are in the form of flakes having a thickness of 0.01 to 0.03 μm, the organic layer has a thickness of 0.5 to 1 μm, and is provided on either the front or back surface of the metal particles, or on both the front and back surfaces.

4. A decorative member according to claim 1, wherein the metal particles of each of the plurality of metal-containing particles are aluminum flake particles.

5. A decorative member according to claim 1, wherein said plurality of metal-containing particles are present only within a depth of 5 μm from the surface of said base material.

6. A decorative member according to claim 1, wherein said plurality of metal-containing particles have an average particle size in the range of 10 to 35 μm.

7. A decorative member according to claim 1, characterized in that said protective coating layer has a thickness of 10 to 50 μm.

8. A decorative member according to claim 1, characterized in that the base material comprises a base and a primer layer provided on the surface of the base material and constituting the surface of the base material.

9. A decorative member according to claim 1, characterized in that a coating film is formed on the surface of said base material between adjacent ones of said plurality of metal-containing particles.

10. A decorative member according to claim 1, characterized in that the attenuation rate of millimeter waves having a frequency in the range of 60 to 90 GHz is in the range of 0.001 to 6 dB, the transmittance of infrared rays having a wavelength in the range of 905 to 1,550 nm is in the range of 80 to 94%, and the L* value (brightness) measured from the side of the base material is in the range of 20 to 80.

11. A decorative member according to claim 1, characterized in that the plurality of metal-containing particles are uniformly scattered across the surface of the substrate when the surface of the substrate is viewed in a plane.

12. A decorative member according to claim 1, characterized in that said protective covering layer is a light-transmitting layer made of a light-transmitting material.

Citation Information

Patent Citations

  • Electromagnetic wave transmissive brilliant coating resin product and its manufacturing method

    JP2010030075A

  • Decorative film

    JP2015080934A

  • Millimeter wave transparent gloss coated film and resin product

    JP2019123819A

  • Infrared transmitting brilliant coating film and infrared transmission cover

    JP2023144247A

  • Electromagnetic wave-permeable laminate

    WO2015033872A1