Coating composition, coating method, and coated body
The coating composition for aluminum alloy wheels, featuring an acrylic resin, crosslinking agent, and silane compound, addresses the challenge of low VOC content and performance by enhancing adhesion, rust prevention, and physical properties, achieving effective scratch resistance and chemical resistance.
Patent Information
- Application Number
- PCT/JP2023/042941
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2023-11-30
- Publication Date
- 2024-10-03
AI Technical Summary
Existing coating compositions for aluminum alloy wheels face challenges in achieving low VOC content while maintaining adhesion, rust prevention, and physical properties such as scratch resistance and chemical resistance, particularly when reduced organic solvent content leads to decreased molecular weight and subsequent performance issues.
A coating composition comprising an acrylic resin with specific hydroxyl group content, a crosslinking agent, and a silane compound with an epoxy group, along with a nitrogen atom-containing monomer, is used to create a coating film with improved adhesion, rust prevention, and physical properties, while minimizing organic solvent content.
The coating composition achieves excellent scratch resistance, coating hardness, and chemical resistance while maintaining low VOC levels, ensuring effective adhesion to metal substrates and preventing rust, even on cut-treated metal surfaces.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Coating composition, coating method, and coated body
[0001] The present invention relates to a coating composition, a coating method, and a coated body.
[0002] Wheels for automobiles and motorcycles are primarily made from aluminum alloys. Castings, in particular, are easily processed into complex shapes, allowing for a variety of designs and mass production. Cast aluminum wheels are machined and then polished, after which a clear coat is applied to the surface to protect the substrate. Clear coating is typically performed sequentially, consisting of a primer clear coat and a top clear coat. As a primer coating, for example, Patent Document 1 discloses an acrylic resin coating containing N-butoxymethylacrylamide as a thermosetting resin and transparent finely powdered silica and / or alumina. Patent Document 2 also discloses a primer coating composition containing a copolymer resin, fumed silica, and a magnesium-containing phosphate compound to improve corrosion resistance. Patent Document 3 also discloses a thermosetting liquid coating composition for aluminum wheels, comprising an acrylic resin obtained by copolymerizing a monomer mixture containing 8 to 40 wt% of a secondary hydroxyl-containing unsaturated monomer, and an amino resin.
[0003] Meanwhile, in recent years, China has been requiring the use of materials that comply with mandatory standards (GB standards) for low-VOC (volatile organic compound) paints, adhesives, etc., and as a result, there is a demand for primer paints with reduced organic solvent content.
[0004] Japanese Patent Application Laid-Open No. 1-194979 International Publication No. 2014 / 181593 International Publication No. 2004 / 094545
[0005] To prepare a paint with a reduced amount of organic solvent, it is necessary to design the resin to have a low viscosity. However, simply lowering the viscosity of the paint by reducing the molecular weight of the resin tends to result in a decrease in the physical properties of the resulting paint film. In particular, primer paints tend to have reduced adhesion to metal substrates and reduced rust prevention properties. Furthermore, aluminum wheels are cleaned with acidic cleaning solutions after production, but their resistance to these solutions tends to be poor. The present invention has been made in consideration of the above circumstances, and a first object thereof is to provide a paint composition having excellent abrasion resistance, coating hardness, and chemical resistance, and a coated body coated with the paint composition. The present invention has been made in consideration of the above circumstances, and a second object thereof is to provide a paint composition having excellent adhesion to metal substrates and rust prevention properties, a coating method using the paint composition, and a coated body coated with the paint composition.
[0006] The first invention is a coating composition (hereinafter sometimes referred to as the first coating composition) comprising an acrylic resin (X) having a total number of hydroxyl groups per number average molecular weight of 2.0 or more and 6.0 or less, a crosslinking agent (Y) that reacts with hydroxyl groups, and an organic solvent (Z), in which the content of the organic solvent (Z) is 600 g / L or less.
[0007] The crosslinking agent (Y) that reacts with a hydroxyl group preferably contains an amino resin.
[0008] It is preferred that the hydroxyl value calculated from the primary hydroxyl groups of the acrylic resin (X) is 40 mgKOH / g or more and 130 mgKOH / g or less, and the ratio of the primary hydroxyl value to the secondary hydroxyl value is 100:0 or more and 100:60 or less.
[0009] The first coated body of the present invention has a coating film formed on a substrate from the first coating composition of the present invention (first coating composition).
[0010] The glass transition temperature Tg of the coating film is preferably 50°C or higher and 98°C or lower.
[0011] The second invention relates to a coating composition (hereinafter sometimes referred to as the second coating composition) which comprises an acrylic resin (A) which contains a nitrogen-atom-containing monomer (a1) as a polymerizable monomer and has an acid value of 15 mgKOH / g or more and 50 mgKOH / g or less, a silane compound (B) having an epoxy group, and an organic solvent (C), wherein the content of the nitrogen-atom-containing monomer (a1) is 5 mass% or more and less than 30 mass% relative to 100 mass% of the total polymerizable monomers, and the content of the organic solvent (C) is 700 g / L or less.
[0012] The nitrogen atom-containing monomer (a1) is preferably a compound having a functional group capable of reacting with a hydroxyl group.
[0013] The number average molecular weight of the acrylic resin (A) is preferably 4,000 or more and 10,000 or less.
[0014] The coating method of the present invention involves coating a metal substrate that has been machined with the second coating composition of the present invention (second coating composition).
[0015] The second coated body of the present invention has a coating film formed from the second coating composition of the present invention (second coating composition) on a machined metal substrate.
[0016] The coated body of the present invention may also have a surface protective layer on the coating film.
[0017] The second coated body of the present invention may further comprise a coating film formed from the first coating composition on top of a coating film formed from the coating composition of the present invention (second coating composition).
[0018] According to the first aspect of the present invention, it is possible to obtain a coating composition having excellent scratch resistance, coating film hardness, and chemical resistance, and a coated body coated with the coating composition. According to the second aspect of the present invention, it is possible to obtain a coating composition, a coating method, and a coated body having excellent adhesion to metal substrates and rust prevention properties.
[0019] First, a first embodiment of the present invention will be described.
[0020] [First Coating Composition] The first coating composition of the present invention is a coating composition containing an acrylic resin (X) having a total number of hydroxyl groups per number average molecular weight of 2.0 to 6.0, a crosslinking agent (Y) that reacts with hydroxyl groups (hereinafter sometimes simply referred to as crosslinking agent (Y)), and an organic solvent (Z), the content of which is 600 g / L or less. Details of each component will be described below.
[0021] <Acrylic Resin (X)> Examples of polymerizable monomers constituting the acrylic resin (X) include one or more acrylic components selected from acrylic acid, methacrylic acid, and esters, amides, and nitriles thereof; and polymerizable unsaturated monomers such as styrene and vinyl group-containing ester compounds (excluding acrylic components).
[0022] (Acrylic Component) Examples of the acrylic component include the following compounds (a1) to (a5).
[0023] —Ester (a1) of (meth)acrylic acid and alcohol having 1 to 24 carbon atoms— Examples of the ester (a1) of (meth)acrylic acid and alcohol having 1 to 24 carbon atoms include methyl (meth)acrylate, 2-isocyanatoethyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, lauryl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, tridecyl (meth)acrylate, and stearyl (meth)acrylate.
[0024] -Carboxyl Group-Containing Monomer (a2)- Examples of the carboxyl group-containing monomer (a2) include acrylic acid, methacrylic acid, maleic acid, and maleic anhydride.
[0025] -Hydroxyl Group-Containing Monomer (a3)- Examples of the hydroxyl group-containing monomer (a3) include monoesters of (meth)acrylic acid with dihydric alcohols, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate, as well as (meth)acrylates having a polyoxyethylene chain with a hydroxyl group at the molecular terminal.
[0026] -Epoxy Group-Containing Polymerizable Unsaturated Monomer (a4)- Examples of the epoxy group-containing polymerizable unsaturated monomer (a4) include glycidyl (meth)acrylate and 3,4-epoxycyclohexylmethyl (meth)acrylate.
[0027] - Aminoalkyl (meth)acrylate (a5) - Examples of the aminoalkyl (meth)acrylate (a5) include N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, and N,N-dimethylaminopropyl (meth)acrylate.
[0028] (Polymerizable Unsaturated Monomer (a6)) Examples of polymerizable monomers other than the acrylic component include the following polymerizable unsaturated monomers (a6): Examples of the polymerizable unsaturated monomer (a6) include vinyl group-containing aromatic compounds such as styrene, α-methylstyrene, and vinyltoluene, and vinyl group-containing compounds such as vinyl acetate.
[0029] (Number average molecular weight Mn) The number average molecular weight Mn of the acrylic resin (X) is 1500 or more and 7500 or less. By having it be 1500 or more, a coating film with good scratch resistance and coating film hardness can be obtained upon crosslinking. By having it be 7500 or less, a coating composition with an organic solvent amount of 600 g / L or less can be obtained. The number average molecular weight Mn of the acrylic resin (X) is preferably 2000 or more and 6000 or less. In this specification, the number average molecular weight Mn of the acrylic resin (X) is measured by the measurement method shown in the examples described later. In the first coating composition of the present invention, by making the number average molecular weight of the acrylic resin (X) relatively low as described above, it is possible to reduce the content of the organic solvent (Z).
[0030] (Hydroxyl value calculated from primary hydroxyl groups) In the acrylic resin (X), the hydroxyl value calculated from the primary hydroxyl groups is preferably 40 mgKOH / g or more and 130 mgKOH / g or less, more preferably 60 mgKOH / g or more and 120 mgKOH / g or less. When the hydroxyl value calculated from the primary hydroxyl groups of the acrylic resin (X) is 40 mgKOH / g or more, sufficient curing to exhibit good coating film performance can be ensured, and scratch resistance and coating film hardness can be ensured. In addition, when the hydroxyl value calculated from the primary hydroxyl groups of the acrylic resin (X) is 130 mgKOH / g or less, unreacted hydroxyl groups can be reduced, resulting in excellent chemical resistance.
[0031] (Hydroxyl value calculated from secondary hydroxyl groups) In the acrylic resin (X), the hydroxyl value calculated from the secondary hydroxyl groups is preferably 40 mg KOH / g or less, more preferably 25 mg KOH / g or less, and even more preferably 10 mg KOH / g or less. When the hydroxyl value calculated from the secondary hydroxyl groups is 40 mg KOH / g or less, a coating film excellent in chemical resistance, scratch resistance, and coating film hardness can be obtained.
[0032] Here, the total hydroxyl value of the acrylic resin (X) is the number of mg of potassium hydroxide required to completely acetylate the hydroxyl groups in 1 g of the resin with acetic anhydride and then neutralize the free acetic acid generated by acetylation.
[0033] (Ratio of primary hydroxyl value to secondary hydroxyl value) Since secondary hydroxyl groups have lower reactivity than primary hydroxyl groups, the balance between the reaction between the acrylic resin (X) and the crosslinking agent (Y) and the reaction between the crosslinking agents (Y) becomes poor, and the chemical resistance, scratch resistance, and coating hardness of the obtained coating film tend to be poor. For this reason, the ratio of the primary hydroxyl value to the secondary hydroxyl value in the acrylic resin (X) is preferably 100:0 or more and 100:60 or less, more preferably 100:0 or more and 100:35 or less.
[0034] (Acid Value) The acid value of the acrylic resin (X) is preferably 10 mgKOH / g or more and 50 mgKOH / g or less. When the acid value is 10 mgKOH / g or more, it is easier to act as a catalyst in the reaction with the amino resin, and a coating film with good scratch resistance and coating hardness can be obtained. When the acid value is 50 mgKOH / g or less, there are few residual acid groups, and a coating film with good chemical resistance can be obtained. In the present invention, the acid value of the acrylic resin (X) is a value determined in accordance with JIS-K-5601-2-1:1999.
[0035] (Total number of hydroxyl groups per number average molecular weight) The total number of hydroxyl groups per number average molecular weight is preferably 2.0 or more and 6.0 or less, more preferably 2.5 or more and 5.5 or less. When the total number of hydroxyl groups per number average molecular weight is 2.0 or more, the number of crosslinking points with the crosslinking agent (Y) increases, curing proceeds well, and a coating film excellent in coating film hardness and scratch resistance can be obtained. Furthermore, when the total number of hydroxyl groups per number average molecular weight is 6.0 or less, the number of residual hydroxyl groups is small, and a coating film excellent in chemical resistance can be obtained. The total number of hydroxyl groups per number average molecular weight is determined by the method described in the Examples below.
[0036] (Weight average molecular weight Mw) The weight average molecular weight Mw of the acrylic resin (X) is preferably 3,000 or more and 18,000 or less. By having it be 3,000 or more, a coating film with good scratch resistance and coating film hardness can be obtained upon crosslinking. By having it be 18,000 or less, a coating composition with an organic solvent amount of 600 g / L or less can be obtained. The weight average molecular weight Mw of the acrylic resin (X) is more preferably 5,000 or more and 14,000 or less. In this specification, the weight average molecular weight Mw of the acrylic resin (X) is measured by the measurement method shown in the examples described later.
[0037] (Total number of hydroxyl groups per weight average molecular weight) The total number of hydroxyl groups per weight average molecular weight is preferably 4.0 or more and 11.0 or less. When the total number of hydroxyl groups per weight average molecular weight is 4.0 or more, the number of crosslinking points with the crosslinking agent (Y) increases, curing proceeds well, and a coating film with good scratch resistance and coating film hardness can be obtained. When the total number of hydroxyl groups per weight average molecular weight is 11.0 or less, the number of residual hydroxyl groups is small, and a coating film with good chemical resistance can be obtained. The total number of hydroxyl groups per weight average molecular weight is determined by the method described in the examples below.
[0038] <Crosslinking Agent (Y) Reactive with Hydroxyl Group> The crosslinking agent (Y) reactive with a hydroxyl group preferably contains an amino resin, and examples of the amino resin include urea resin, melamine resin, and benzoguanamine resin.
[0039] (Mass ratio of acrylic resin (X) / crosslinking agent (Y) reactive with hydroxyl groups) The mass ratio of the acrylic resin (X) to the crosslinking agent (Y) reactive with hydroxyl groups, "acrylic resin (X) / crosslinking agent (Y) reactive with hydroxyl groups," is preferably 60 / 40 or more and 75 / 25 or less, and more preferably 60 / 40 or more and 70 / 30 or less. By adjusting the acrylic resin (X) / crosslinking agent (Y) reactive with hydroxyl groups within the above range, a coating film with good coating film hardness, scratch resistance, and chemical resistance can be obtained.
[0040] <Organic Solvent (Z)> Examples of the organic solvent (Z) include butyl acetate, xylene, ethylene glycol mono-normal propyl ether, toluene, methyl isobutyl ketone, isopropyl alcohol, butanol, acetone, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, methyl ethyl ketone, ethyl 3-ethoxypropionate, aromatic solvents (e.g., Solvesso 150, toluene, xylene), etc. Known commercially available products can be used as these solvents.
[0041] The content of organic solvent (Z) in the first coating composition of the present invention is 600 g / L or less. In the first coating composition of the present invention, the content of organic solvent (Z) can be further reduced to 550 g / L or less, or even 450 g / L or less. When the content of organic solvent (Z) is 600 g / L or less, the coating composition can be applied without dilution. Furthermore, in the first invention, even if a coating composition with an even lower content of organic solvent (Z), such as 430 g / L or less, is prepared and then diluted immediately before application to a viscosity suitable for application, the content of organic solvent (Z) in the coating composition at the time of application can be reduced to 600 g / L or less. Therefore, the first coating composition of the present invention is an environmentally friendly coating composition. Furthermore, even when the content of organic solvent (Z) in the first coating composition of the present invention is as low as described above, it exhibits good curability and excellent abrasion resistance, coating film hardness, and chemical resistance.
[0042] The concentration of the organic solvent (Z) in the first coating composition of the present invention is preferably 35% by mass or more and 55% by mass or less, from the viewpoint of coatability and environmental considerations.
[0043] <Other Components> The first coating composition of the present invention can appropriately use additives necessary for a coating composition. For example, various coating additives that are generally known and commonly used in the art, such as pigments, pigment dispersants, antifoaming agents, anti-sagging agents, UV absorbers, light stabilizers, and anti-fungal agents, can be used in conventional amounts. Furthermore, the first coating composition of the present invention can also be appropriately used in combination with other resins, such as acrylic-modified alkyd resins, alkyd resins, silicone resins, fluororesins, and epoxy resins, for the purpose of improving performance within a range that does not affect the effects of the present invention.
[0044] <Total Light Transmittance> The first coating composition of the present invention is preferably a clear coating composition from the viewpoint of application to highly decorative substrates. In this specification, a clear coating composition is a coating composition that forms a transparent coating film, and when the coating film has a thickness of 30 μm, the transmittance is 80% or more, preferably 90% or more, more preferably 95% or more, and even more preferably 97% or more. In this specification, transmittance refers to the total light transmittance in the visible region (360 nm to 750 nm) and can be measured in accordance with JIS K 7375:2008.
[0045] [Properties of Coating Film] The properties of the coating film formed using the first coating composition of the present invention will be described below.
[0046] <Water Contact Angle of Coating Film> The water contact angle of the coating film obtained by coating to a dry film thickness of 30 μm is preferably 80° or more. If the water contact angle on the coating film surface is 80° or more, penetration of hydrophilic components into the coating film is more easily suppressed.
[0047] <Crosslink Density of Coating Film> The crosslink density of the coating film is preferably 0.00050 mol / cc or more and 0.00180 mol / cc or less, and more preferably 0.00077 mol / cc or more and 0.00125 mol / cc or less. By adjusting the crosslink density of the coating film within the above range, a coating film with good coating film hardness, scratch resistance, and chemical resistance can be obtained.
[0048] <Molecular weight between crosslinks of coating film (1 / crosslink density)> The molecular weight between crosslinks of the coating film (1 / crosslink density) is preferably 550 cc / mol or more and 2000 cc / mol or less, and more preferably 800 cc / mol or more and 1300 cc / mol or less. By adjusting the molecular weight between crosslinks of the coating film (1 / crosslink density) to within the above range, a coating film with good coating film hardness, scratch resistance, and chemical resistance can be obtained.
[0049] <Glass transition temperature Tg of coating film> The glass transition temperature Tg of a coating film obtained by coating to a dry film thickness of 30 μm is preferably 50° C. or higher and 98° C. or lower, and more preferably 65° C. or higher and 95° C. or lower. When the glass transition temperature Tg of the coating film is 50° C. or higher, a coating film excellent in abrasion resistance and coating film hardness can be obtained. When the glass transition temperature Tg is 98° C. or lower, a coating film excellent in chemical resistance can be obtained.
[0050] <Coating film hardness> The coating film preferably has a hardness of 2B or more, more preferably HB or more, measured in accordance with JIS K5600 5-3:1999 scratch hardness (pencil method). With such a coating film hardness, even when used on metal substrates (e.g., aluminum wheels of automobiles, etc.), the design can be maintained for a long period of time, thereby providing high quality.
[0051] [Coating method] The coating method of the present invention involves coating a substrate with the first coating composition of the present invention. Coating methods include, for example, dipping, electrostatic coating, spin coating, flow coating, roll coating, spray coating, blade coating, and air knife coating. Among these, spray coating and roll coating are preferred from the viewpoint of easy control of film thickness.
[0052] The reaction of the coating film formed by applying the first coating composition is not yet complete at the time of coating film formation, and the drying and curing reaction are terminated by baking (heat drying) to cause a curing reaction after the coating film is formed. The baking conditions are preferably 80 to 180°C for 5 to 90 minutes.
[0053] <Substrate> The substrate in the first invention is not particularly limited, and its shape may be, for example, plate-like, sheet-like, foil-like, etc. Furthermore, metal substrates include steel, galvanized steel, stainless steel, magnesium alloys, aluminum, aluminum alloys, etc., with aluminum alloys being preferred. The metal substrate may be subjected to various surface treatments, such as oxidation treatment. As an example, a substrate in which aluminum has been subjected to oxidation treatment using methods such as anodizing, phosphate treatment, chromate treatment, and non-chromate treatment can be used. In addition, the metal substrate may be coated with an electrodeposition coating or primer, or the first coating composition of the present invention may be applied to a metal substrate on which a decorative layer has been formed. The decorative layer can be formed using paint, ink, vapor deposition, etc., and may be a metallic decorative layer. Furthermore, the paint and ink used to form the decorative layer may be solvent-based, water-based, or solvent-free, and paints and inks that cure using heat or active energy rays can also be used. The first coating composition of the present invention is useful as a top clear coating for metal substrates, and the coating film formed therefrom exhibits excellent scratch resistance, coating film hardness, and chemical resistance.
[0054] [Coated body] The first coated body of the present invention has a coating film formed on a substrate from the first paint composition of the present invention. The coating film can be formed by the coating method described above. Because the first coated body of the present invention has a coating film formed from the first paint composition, it has excellent scratch resistance, coating film hardness, and chemical resistance. Furthermore, the first coated body of the present invention may further have a surface protective layer on the coating film that has properties such as contamination resistance.
[0055] Next, a second embodiment of the present invention will be described.
[0056] [Second coating composition] The second coating composition of the present invention contains an acrylic resin (A) containing a nitrogen atom-containing monomer (a1) as a polymerizable monomer and having an acid value of 15 mg KOH / g or more and 50 mg KOH / g or less, an epoxy group-containing silane compound (B), and an organic solvent (C), wherein the content of the nitrogen atom-containing monomer (a1) in the acrylic resin (A) is 5 mass% or more and less than 30 mass%, and the content of the organic solvent (C) is 700 g / L or less. Details of each component will be explained below.
[0057] <Acrylic Resin (A)> The acrylic resin (A) contains at least a nitrogen-atom-containing monomer (a1) as a polymerizable monomer. In addition to the nitrogen-atom-containing monomer (a1), the polymerizable monomer constituting the acrylic resin (A) may include one or more acrylic components selected from acrylic acid, methacrylic acid, and esters thereof; and polymerizable unsaturated monomers such as styrene and vinyl group-containing compounds (excluding acrylic components).
[0058] (Nitrogen Atom-Containing Monomer (a1)) The nitrogen atom-containing monomer (a1) is preferably a compound having a functional group capable of reacting with a hydroxyl group. Examples of the nitrogen atom-containing monomer (a1) include (meth)acrylamide and derivatives thereof, more specifically, (meth)acrylamide, N,N-dimethylaminoethyl(meth)acrylamide, N,N-diethylaminoethyl(meth)acrylamide, N-methoxymethylacrylamide, N-butoxymethylacrylamide, N-isobutoxymethylacrylamide, N-dimethylaminopropyl(meth)acrylamide, and N-methylolacrylamide.
[0059] The content of the nitrogen atom-containing monomer (a1) is 5% by mass or more and less than 30% by mass, based on 100% by mass of all polymerizable monomers. When the content of the nitrogen atom-containing monomer (a1) is 5% by mass or more, adhesion to metal substrates is improved. Furthermore, when the content of the nitrogen atom-containing monomer (a1) is less than 30% by mass, high rust prevention properties can be obtained. The content of the nitrogen atom-containing monomer (a1) is more preferably 5% by mass or more and 25% by mass or less, based on 100% by mass of all polymerizable monomers.
[0060] (Acrylic Component) Examples of the acrylic component of the polymerizable monomer include the following compounds (a2) to (a6).
[0061] —Ester (a2) of (meth)acrylic acid and alcohol having 1 to 24 carbon atoms— Examples of the ester (a2) of (meth)acrylic acid and alcohol having 1 to 24 carbon atoms include methyl (meth)acrylate, 2-isocyanatoethyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, lauryl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, tridecyl (meth)acrylate, and stearyl (meth)acrylate.
[0062] -Carboxyl Group-Containing Monomer (a3)- Examples of the carboxyl group-containing monomer (a3) include acrylic acid, methacrylic acid, maleic acid, and maleic anhydride.
[0063] -Hydroxyl Group-Containing Monomer (a4)- Examples of the hydroxyl group-containing monomer (a4) include monoesters of (meth)acrylic acid with dihydric alcohols, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate, as well as (meth)acrylates having a polyoxyethylene chain with a hydroxyl group at the molecular terminal.
[0064] -Epoxy Group-Containing Polymerizable Unsaturated Monomer (a5)- Examples of the epoxy group-containing polymerizable unsaturated monomer (a5) include glycidyl (meth)acrylate and 3,4-epoxycyclohexylmethyl (meth)acrylate.
[0065] (Polymerizable Unsaturated Monomer (a6)) Examples of polymerizable monomers other than the acrylic component include the following polymerizable unsaturated monomers (a6): Examples of the polymerizable unsaturated monomer (a6) include vinyl group-containing aromatic compounds such as styrene, α-methylstyrene, and vinyltoluene, vinyl group-containing compounds such as vinyl acetate, and vinyl group-containing ester compounds.
[0066] (Hydroxyl value) The hydroxyl value of the acrylic resin (A) is preferably 10 mgKOH / g or more and 80 mgKOH / g or less. When the hydroxyl value of the acrylic resin (A) is 10 mgKOH / g or more, the crosslinking reaction with the nitrogen atom-containing monomer proceeds easily, and a coating film having a dense crosslinked structure with excellent rust prevention properties can be obtained. When the hydroxyl value is 80 mgKOH / g or less, the crosslinking reaction with the nitrogen atom-containing monomer reduces unreacted hydroxyl groups, and a coating film with excellent rust prevention properties can be obtained. The hydroxyl value of the acrylic resin (X) is the number of mg of potassium hydroxide required to completely acetylate the hydroxyl groups in 1 g of resin with acetic anhydride and then neutralize the free acetic acid generated by acetylation.
[0067] (Acid Value) The acid value of the acrylic resin (A) is 15 mgKOH / g or more and 50 mgKOH / g or less. When the acid value is 15 mgKOH / g or more, the crosslinking reaction of the nitrogen atom-containing monomer is facilitated, and a coating film with good adhesion to the metal substrate can be obtained. When the acid value is 50 mgKOH / g or less, the amount of residual acid groups remaining after the reaction with the silane compound (B) having an epoxy group is reduced, and a coating film with good rust prevention properties can be obtained. In the present invention, the acid value of the acrylic resin (A) is a value determined in accordance with JIS K 5601-2-1:1999.
[0068] (Number average molecular weight Mn) The number average molecular weight Mn of the acrylic resin (A) is preferably 4000 or more and 10000 or less. When it is 4000 or more, a coating film having good adhesion to the metal substrate can be obtained as a coating film of a high molecular weight substance after the crosslinking reaction, and when it is 10000 or less, an acrylic resin with low viscosity can be obtained, so that the organic solvent content in the coating material can be 700 g / L or less. In this specification, the number average molecular weight Mn of the acrylic resin (A) is measured by the measurement method shown in the examples described later.
[0069] (Weight average molecular weight Mw) The weight average molecular weight Mw of the acrylic resin (A) is preferably 10,000 or more and 40,000 or less. When it is 10,000 or more, a coating film with good adhesion to the metal substrate can be obtained as a coating film of a high molecular weight substance after the crosslinking reaction, and when it is 40,000 or less, an acrylic resin with low viscosity can be obtained, so that the organic solvent content in the coating material can be 700 g / L or less. In this specification, the weight average molecular weight Mw of the acrylic resin (A) is measured by the measurement method shown in the examples described later.
[0070] (Glass Transition Temperature Tg) The glass transition temperature Tg of the acrylic resin (A) is preferably −40° C. or higher and 50° C. or lower. When the glass transition temperature Tg is in this range, adhesion to metal substrates and rust prevention properties tend to be improved.
[0071] <Silane Compound (B) Having an Epoxy Group> As the silane compound (B) having an epoxy group, compounds known as epoxy group-containing silane coupling agents can be used. Examples include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltriethoxysilane. By containing the silane compound (B) having an epoxy group, the second coating composition of the present invention can improve the adhesion and rust prevention between the coating film formed and the metal substrate.
[0072] <Organic Solvent (C)> Examples of the organic solvent (C) include xylene, ethylene glycol mono-normal propyl ether, toluene, methyl isobutyl ketone, isopropyl alcohol, butanol, acetone, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, methyl ethyl ketone, ethyl 3-ethoxypropionate, etc. Known commercially available products can be used as these solvents.
[0073] The content of organic solvent (C) in the second coating composition of the present invention is 700 g / L or less. In the second coating composition of the present invention, the content of organic solvent (C) can be further reduced to 650 g / L or less, more preferably 600 g / L or less. When the content of organic solvent (C) is 700 g / L or less, spray coating is possible without diluting the coating composition. When a coating is spray-coated, the coating is required to have a low viscosity. In the present invention, when a coating composition is provided with an even lower content of organic solvent (C), for example, 430 g / L or less, even when diluted to a level that allows spray coating, the concentration of organic solvent (C) can be reduced to 700 g / L or less. Therefore, the second coating composition of the present invention is an environmentally friendly coating composition. Furthermore, even when the content of organic solvent (C) in the second coating composition of the present invention is as low as described above, the adhesion of the coating to metal substrates and the rust prevention properties of the coating film are not reduced.
[0074] <Other Components> The second coating composition of the present invention can appropriately use additives necessary for a coating composition. For example, various coating additives that are generally known and commonly used in the art, such as pigments, pigment dispersants, antifoaming agents, anti-sagging agents, UV absorbers, light stabilizers, and anti-fungal agents, can be used in conventional amounts. Furthermore, the second coating composition of the present invention can also be appropriately used in combination with other resins, such as acrylated alkyd resins, alkyd resins, silicone resins, fluororesins, and epoxy resins, for the purpose of improving performance within a range that does not affect the effects of the present invention.
[0075] <Total Light Transmittance> When the second coating composition of the present invention is used as a clear coating, the total light transmittance of the coating film obtained by applying it so that the dry film thickness is 25 μm is preferably 90% or more.
[0076] [Coating method] The second coating method of the present invention involves coating a metal substrate that has been machined with the second coating composition of the present invention. Coating methods include, for example, dipping, electrostatic coating, spin coating, flow coating, roll coating, spray coating, blade coating, and air knife coating. Among these, spray coating and roll coating are preferred from the viewpoint of easy control of film thickness.
[0077] The reaction of the coating film formed by applying the second coating composition is not yet complete at the time of coating film formation, and the drying and curing reaction are terminated by baking (heat drying) to cause a curing reaction after the coating film is formed. The baking conditions are preferably 80 to 180°C for 5 to 90 minutes.
[0078] <Machine-treated metal substrate> The "metal substrate" of the machined metal substrate in the second invention is not particularly limited, and its shape may be, for example, plate-like, sheet-like, foil-like, etc. In addition, metals constituting the metal substrate include steel, galvanized steel, stainless steel, magnesium alloy, aluminum, aluminum alloy, etc., among which aluminum alloy is preferred. In particular, the effect of the second coating composition of the present invention is more pronounced when it is used on aluminum alloy castings, which are widely used for automobile wheels. That is, for automobile wheels, machining is performed to impart gloss, and there is a problem that machined metal surfaces are prone to rust. However, when the second coating composition of the present invention is applied to a machined metal substrate, it has good adhesion and rust prevention properties. The effect of the second coating composition of the present invention is more pronounced when applied to a machined metal substrate, but of course, the effect of the second coating composition of the present invention is also fully exerted even on metal substrates that have not been machined.
[0079] The metal substrate may be subjected to various surface treatments, such as oxidation treatment. For example, a substrate can be used in which aluminum is subjected to oxidation treatment by a method such as anodizing, phosphate treatment, chromate treatment, or non-chromate treatment.
[0080] [Coated body] The second coated body of the present invention has a coating film formed from the second paint composition of the present invention on a machined metal substrate. The coating film can be formed by the second coating method of the present invention described above. Since the second coated body of the present invention is coated with the second paint composition of the present invention, it has good adhesion between the metal substrate and the coating film and excellent rust prevention properties. The second coated body of the present invention may have a surface protective layer on the coating film.
[0081] [Surface Protective Layer] A typical topcoat paint can be used as the paint for forming the surface protective layer, but it is preferable to use a paint that can form a coating film that is excellent in abrasion resistance, coating film hardness, and chemical resistance. A coating film with excellent abrasion resistance may also be a coating film that has self-repairing properties even if scratches occur on the coating film. Examples of paints that can form a coating film with excellent coating film hardness and chemical resistance include thermosetting paints and active energy ray-curable paints such as acrylic melamine resin paints and acrylic urethane resin paints. The surface protective layer formed on the coating film formed from the second coating composition of the present invention is preferably formed from an acrylic melamine resin paint or acrylic urethane resin paint containing a nitrogen atom-containing resin component, and in particular, an acrylic melamine resin paint is more preferred. The paint for forming the surface protective layer is preferably an acrylic resin (X) having a total hydroxyl group number per number average molecular weight of 2.0 to 6.0, a crosslinking agent (Y) that reacts with hydroxyl groups, and an organic solvent (Z), and the content of the organic solvent (Z) is more preferably 600 g / L or less. Such a paint can form a coating film that is excellent in abrasion resistance, coating film hardness, and chemical resistance, while being a low-VOC (volatile organic compound) paint. Furthermore, the surface protective layer is preferably a clear paint from the viewpoint of application to highly decorative substrates. In this specification, a clear paint is a paint that forms a transparent coating film, and when the thickness is 30 μm, the paint forms a coating film with a transmittance of 80% or more, preferably 90% or more, more preferably 95% or more, and even more preferably 97% or more. In this specification, transmittance refers to the total light transmittance in the visible region (360 nm to 750 nm) and can be measured in accordance with JIS K 7375:2008.
[0082] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the examples shown below.
[0083] A first embodiment of the present invention will be described.
[0084] [Preparation of Acrylic Resin Solution] First, a resin solution containing acrylic resin (X) was prepared for use in the Examples and Comparative Examples. [Resin Solution T1] Resin solution T1 containing acrylic resin (X) was prepared according to the following procedure. Table 1 shows the monomers and solvents required for resin preparation, as well as the properties of acrylic resin (X). 30.0 parts by mass of xylene, 31.0 parts by mass of styrene, 12.0 parts by mass of 2-ethylhexyl acrylate, 43.0 parts by mass of 2-ethylhexyl methacrylate, 2.0 parts by mass of acrylic acid, 12 parts by mass of 2-hydroxyethyl methacrylate, and 4.0 parts by mass of 2-2'-azobis-2-methylbutyronitrile were reacted for 8 hours at 100°C under nitrogen gas. The mixture was then diluted with 32.7 parts by mass of xylene to obtain acrylic resin solution T1 with a heating residue of 60% by mass.
[0085] The acrylic resin (X) contained in the acrylic resin solution T1 had a hydroxyl value of 45 mgKOH / g, an acid value of 11 mgKOH / g, a number average molecular weight of 3,500, and a weight average molecular weight of 6,000.
[0086] [Resin Solutions T2 to T21] Resin solutions T2 to T21 were prepared in the same manner as resin solution T1, except that the compounds and formulations were changed as shown in Tables 1 to 3.
[0087] (Heating residue) 1.0 g of the resin solution was precisely weighed into an aluminum cup and dried for 30 minutes in an oven at 150° C. After drying, the mass of the residue was precisely weighed, and the ratio of the mass of the residue to the original mass was calculated as the heating residue (mass %).
[0088] (Hydroxyl value) After the hydroxyl groups in 1 g of acrylic resin (X) were completely acetylated with acetic anhydride, the number of mg of potassium hydroxide required to neutralize the free acetic acid generated by the acetylation was determined, and this value was taken as the hydroxyl value of the acrylic resin (X).
[0089] (Acid Value) The acid value of the acrylic resin (X) was determined in accordance with JIS-K-5601-2-1:1999.
[0090] (Number Average Molecular Weight Mn) The number average molecular weight Mn of the acrylic resin (X) was measured using a TSKgel column SuperMultipore HZ-M (manufactured by Tosoh Corporation) by SEC (size exclusion chromatography, trade name "HLC-8420GPC", manufactured by Tosoh Corporation) equipped with a differential refractive index (RI) detector. The SEC conditions were tetrahydrofuran as the developing solvent, a flow rate of 0.35 ml / min, and a temperature of 40°C. TSK standard polystyrene (manufactured by Tosoh Corporation) was used as the standard substance.
[0091] (Weight-average molecular weight Mw) The weight-average molecular weight Mw of the acrylic resin (X) was measured using a TSKgel column SuperMultipore HZ-M (manufactured by Tosoh Corporation) by SEC (size exclusion chromatography, product name "HLC-8420GPC", manufactured by Tosoh Corporation) equipped with a differential refractive index (RI) detector. The SEC conditions were tetrahydrofuran as the developing solvent, a flow rate of 0.35 ml / min, and a temperature of 40°C. TSK standard polystyrene (manufactured by Tosoh Corporation) was used as the standard substance.
[0092] (Glass Transition Temperature Tg of Acrylic Resin (X)) The glass transition temperature Tg of the acrylic resin (X) was calculated by Fox's formula.
[0093] (Total Number of Hydroxyl Groups per Number Average Molecular Weight Mn of Acrylic Resin (X)) The total number of hydroxyl groups per number average molecular weight Mn of acrylic resin (X) was calculated from the measurement result of the number average molecular weight Mn and the value of the hydroxyl value according to the following formula (1): "Total number of hydroxyl groups per number average molecular weight Mn" = number average molecular weight of acrylic resin × (hydroxyl value of acrylic resin (mg KOH / g) / 56100) ... (1)
[0094] (Total Number of Hydroxyl Groups per Weight Average Molecular Weight Mw of Acrylic Resin (X)) The total number of hydroxyl groups per weight average molecular weight Mw of acrylic resin (X) was calculated from the measurement results of the weight average molecular weight Mw and the value of the hydroxyl value according to the following formula (2): "Total number of hydroxyl groups per weight average molecular weight Mw" = Weight average molecular weight of acrylic resin × (Hydroxyl value of acrylic resin (mg KOH / g) / 56100) (2)
[0095] (Ratio of Primary Hydroxyl Value to Secondary Hydroxyl Value) The ratio of the primary hydroxyl value to the secondary hydroxyl value of the acrylic resin (X) was calculated by calculating the theoretical primary hydroxyl value and the theoretical secondary hydroxyl value, respectively, and then calculating the ratio.
[0096]
[0097]
[0098]
[0099] Next, using the above resin solution, coating compositions of Examples and Comparative Examples and coated bodies provided with coating films formed by applying and curing the coating compositions were prepared. The components used in the coating compositions and their formulations are shown in Tables 4 to 6. In Tables 4 to 6, the amount of each component used is expressed in parts by mass.
[0100] [Example 1-1] (Preparation of Coating Composition) 61.7 parts by mass of resin solution T1 was used as the acrylic resin (X), 26.5 parts by mass of a melamine resin solution (a xylene / n-butanol mixed solution of n-butylated melamine resin (heating residue 60% by mass), trade name: AMIDIR L-117-60, manufactured by DIC Corporation) was used as the crosslinking agent (Y) reactive with hydroxyl groups, 3.0 parts by mass of propylene glycol monomethyl ether acetate, 1.0 part by mass of butyl acetate, and 2.8 parts by mass of Solvesso 150 (manufactured by JX Nippon Oil & Energy Corporation) were used as the organic solvent (Z), 1.0 part by mass of a hydroxyphenyltriazine-based ultraviolet absorber (trade name: TINUVIN400, manufactured by BASF) was used as the ultraviolet absorber, and 1.0 part by mass of a hindered amine-based light stabilizer (trade name: EVERSORB93, EVERLIGHT) was used as the light stabilizer. The coating composition of Example 1-1 was prepared by mixing 1.0 part by mass of methyl orthoacetate (trade name: MOA, manufactured by Nippoh Chemical Co., Ltd.) as a dehydrating agent and 3.0 parts by mass of methyl orthoacetate (trade name: MOA, manufactured by Nippoh Chemical Co., Ltd.) as a dehydrating agent, followed by stirring with a disperser.
[0101] (Preparation of Coated Body (Substrate: Aluminum)) The above coating composition was spray-coated onto a substrate made of aluminum, 0.8 mm thick, and 150 mm x 70 mm in size, to a dry film thickness of 30 μm, and then the coating composition was dried at 140° C. for 20 minutes to form a coating film, thereby preparing a coated body (substrate: aluminum). This coated body was used to evaluate chemical resistance, scratch resistance, and coating film hardness.
[0102] (Preparation of Coated Body (Substrate: Polypropylene)) The above coating composition was spray-coated onto a substrate made of polypropylene, 3.0 mm thick, and 100 mm x 100 mm in size, to a dry film thickness of 30 μm, and then the coating composition was dried at 140° C. for 20 minutes to form a coating film, thereby preparing a coated body (substrate: polypropylene). This coated body was used to measure the glass transition temperature Tg, inter-crosslink molecular weight, and crosslink density of the coating film.
[0103] [Examples 1-2 to 1-14, Comparative Examples 1-1 to 1-10] Coating compositions were prepared in the same manner as in Example 1, except that the resin solution containing the acrylic resin (X) was changed as shown in Tables 4 to 6.
[0104] [Evaluation] The coated bodies of the above Examples and Comparative Examples were evaluated as follows. The evaluation results are shown in Tables 4 to 6.
[0105] (Ford Cup Viscosity in Seconds During Application) The flow time of the coating composition during application was measured at 20° C. using a Ford Cup #4 according to JIS K5600-2-2:1999.
[0106] (Glass Transition Temperature Tg of Coating Film) The coating films of Examples 1-1 to 1-14 and Comparative Examples 1-1 to 1-10 were peeled from the polypropylene resin plates and then cut into a sample length of 50 mm and width of 8 mm to prepare measurement samples. The samples were subjected to dynamic viscoelasticity measurement using a dynamic viscoelasticity measuring device RSA G2 (manufactured by TA Instruments) at a measurement length of 24 mm, a frequency of 1 Hz, and a heating rate of 5°C / min. The dynamic glass transition temperature measured as the temperature showing the maximum value of tan δ (loss modulus / storage modulus) was taken as the glass transition temperature.
[0107] (Inter-crosslink molecular weight and crosslink density of coating film) The molecular weight of the resin between crosslinks is called the inter-crosslink molecular weight, and is expressed as the reciprocal of the crosslink density; this value decreases as the crosslink density increases. The inter-crosslink molecular weight of the cured coating film of the present invention is a theoretically calculated value obtained by applying the minimum value of the storage modulus obtained when measuring the glass transition temperature of the cured coating film to the following theoretical formula of rubber viscoelasticity. Formula 1: n = E' / 3RT Where, n: crosslink density (mol / cc) 1 / n: inter-crosslink molecular weight (cc / mol) R: gas constant (8.314 J / K / mol) T: absolute temperature (K) when the storage modulus is E' E': minimum value of the storage modulus (Pa)
[0108] (Chemical Resistance) 1 ml of an aqueous solution of hydrofluoric acid (10% hydrofluoric acid) was dropped onto the surface of the coating film of Examples 1-1 to 1-14 and Comparative Examples 1-1 to 1-10, and then the coating film was left in a test tank without forced convection at a temperature of 23°C for 2 hours for chemical treatment. The aqueous solution of hydrofluoric acid was then removed by rinsing with water, and the appearance of the coating film after chemical treatment was visually evaluated according to the following evaluation criteria. - Evaluation Criteria - AA: No change in the appearance of the coating film. A: The gloss of the coating film is slightly reduced. C: The gloss of the coating film is significantly reduced.
[0109] (Coating film hardness) The coating films of Examples 1-1 to 1-14 and Comparative Examples 1-1 to 1-10 were measured according to "JIS K5600-5-4:1999 Scratch hardness (pencil method)" and evaluated according to the following evaluation criteria. -Evaluation criteria- AA: Pencil hardness is HB or higher A: Pencil hardness is 2B or higher and B or lower C: Pencil hardness is 3B or lower
[0110] (Abrasion resistance) Using a friction fastness tester (manufactured by Daiei Kagaku Seiki Co., Ltd.), a white cloth attached for dye fastness testing in accordance with JIS L 0849 was rubbed back and forth 10 times with a load of 1 kg applied to the coating surface of the coated body. After 10 times of rub-back, the coating surface was washed with running water and allowed to dry naturally, after which the gloss of the coating was visually observed and rated according to the following evaluation criteria: AA: No change in gloss; A: Very slight gloss fade; C: Significant gloss fade
[0111]
[0112]
[0113]
[0114] As shown in Tables 4 to 6, the coating films of Examples 1-1 to 1-14, which used the first coating composition of the present invention, were excellent in abrasion resistance, coating hardness, and chemical resistance. Comparative Examples 1-1 and 1-2, which used resin solutions T13 and T14, each having a total hydroxyl group number per number-average molecular weight ranging from 1.1 to 1.4, were inferior in both abrasion resistance and coating hardness. Comparative Examples 1-3 to 1-8, which used resin solutions T15 to T20, each having a total hydroxyl group number per number-average molecular weight ranging from 6.4 to 7.5, were inferior in chemical resistance. Furthermore, Comparative Example 1-9, which used resin solution T21, whose total hydroxyl group number per number-average molecule was 0, was inferior in both abrasion resistance and coating hardness. Furthermore, Comparative Example 1-10, which did not contain the melamine resin crosslinker, was inferior in chemical resistance, abrasion resistance, and coating hardness.
[0115] Next, a second embodiment of the present invention will be described.
[0116] [Preparation of Acrylic Resin Solution] First, a resin solution containing the acrylic resin (A) used in the examples and comparative examples was prepared. [Resin Solution P1] A solution containing the acrylic resin (A) (resin solution P1) was prepared according to the following procedure. Table 7 shows the monomers and solvents required for preparing the resin solution, as well as the properties of the acrylic resin (A). 30.0 parts by mass of xylene, 35.0 parts by mass of styrene, 45.3 parts by mass of 2-ethyl acrylate, 4.7 parts by mass of methacrylic acid, 10.0 parts by mass of 2-hydroxyethyl methacrylate, 5.0 parts by mass of N-butoxymethyl acrylamide, and 1.5 parts by mass of 2-2'-azobis-2-methylbutyronitrile were reacted under nitrogen gas at 100°C for 8 hours, and then diluted with 50.3 parts by mass of xylene to obtain acrylic resin solution P1 with a heating residue of 55% by mass.
[0117] The acrylic resin (A) contained in the acrylic resin solution P1 had a hydroxyl value of 40 mgKOH / g, an acid value of 30 mgKOH / g, a number average molecular weight of 9,500, and a weight average molecular weight of 35,000.
[0118] [Resin Solutions P2 to P7] Resin solutions P2 to P7 were prepared in the same manner as resin solution P1, except that the compounds and formulations were changed as shown in Table 7.
[0119] The resin properties of resin solutions P1 to P7 were measured by the following methods. The measurement results are shown in Table 7.
[0120] (Heating residue) 1.0 g of the resin solution was precisely weighed into an aluminum cup and dried for 30 minutes in an oven at 150° C. After drying, the mass of the residue was precisely weighed, and the ratio of the mass of the residue to the original mass was calculated as the heating residue (mass %).
[0121] (Hydroxyl value) After the hydroxyl groups in 1 g of acrylic resin (A) were completely acetylated with acetic anhydride, the number of mg of potassium hydroxide required to neutralize the remaining free acetic acid was determined, and this value was taken as the hydroxyl value of the acrylic resin (A).
[0122] (Acid Value) The acid value of the acrylic resin (A) was determined in accordance with JIS K 5601-2-1:1999.
[0123] (Number Average Molecular Weight Mn) The number average molecular weight Mn of the acrylic resin (A) was measured using a TSKgel column SuperMultipore HZ-M (manufactured by Tosoh Corporation) by SEC (size exclusion chromatography, product name "HLC-8420GPC", manufactured by Tosoh Corporation) equipped with a differential refractive index (RI) detector. The SEC conditions were tetrahydrofuran as the developing solvent, a flow rate of 0.35 ml / min, and a temperature of 40°C. TSK standard polystyrene (manufactured by Tosoh Corporation) was used as the standard substance.
[0124] (Weight-average molecular weight Mw) The weight-average molecular weight Mw of the acrylic resin (A) was measured using a TSKgel column SuperMultipore HZ-M (manufactured by Tosoh Corporation) by SEC (size exclusion chromatography, product name "HLC-8420GPC", manufactured by Tosoh Corporation) equipped with a differential refractive index (RI) detector. The SEC conditions were tetrahydrofuran as the developing solvent, a flow rate of 0.35 ml / min, and a temperature of 40°C. TSK standard polystyrene (manufactured by Tosoh Corporation) was used as the standard substance.
[0125]
[0126] Next, using the resin solutions P1 to P7, the coating compositions of the examples and comparative examples and coated bodies provided with coating films formed by applying and curing the coating compositions were prepared. The components used in the coating compositions and their formulations are shown in Table 8. In Table 8, the amount of each component used is expressed in parts by mass.
[0127] [Example 2-1] (Preparation of coating composition) As the acrylic resin (A), 92.6 parts by mass of resin solution P1, as the silane compound having an epoxy group (B), 2.0 parts by mass of KBM-403 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), as the organic solvent (C), 4.0 parts by mass of butyl acetate and 30.0 parts by mass of xylene, as an ultraviolet absorber, 1.0 part by mass of a hydroxyphenyltriazine ultraviolet absorber (trade name: TINUVIN400, manufactured by BASF Corporation), and 1.0 part by mass of a hindered amine light stabilizer (trade name: EVERSORB93, manufactured by EVERLIGHT CHEMICAL Co., Ltd.) as a light stabilizer, were mixed and stirred with a disperser to prepare the coating composition of Example 2-1.
[0128] (Preparation of Coated Body) The above coating composition was air spray coated onto a substrate made of aluminum, having a thickness of 0.8 mm and a size of 150 mm x 70 mm, so that the dry film thickness was 25 μm, and then the coating composition was dried at 140° C. for 20 minutes to prepare a coated body.
[0129] (Ford cup viscosity in seconds during application) The flow time of the coating composition during application was measured at 20° C. using a Ford cup #4 according to a method in accordance with JIS K5600-2-2:1999.
[0130] [Examples 2-2 to 2-4, Comparative Examples 2-1 to 2-5] Except for changing the resin solution containing the acrylic resin (A) as shown in Table 8, coating compositions were prepared in the same manner as in Example 2-1, and coated bodies were produced.
[0131] [Evaluation] The coated bodies of the above Examples and Comparative Examples were evaluated as follows. The evaluation results are shown in Table 8.
[0132] (Adhesion) According to the test method of JIS K 5600-5-6:1999, a coated plate was immersed in deionized water at 40°C for 240 hours, and then 100 2mm grids were made on the coating film using a cutter knife, and a cellophane tape peeling test was performed, after which the adhesion was visually evaluated according to the following criteria. - Evaluation criteria - A: No peeling was observed in any of the 100 grids B: 95 to 99 of the 100 grids remained C: Peeling was observed in 6 or more of the 100 grids
[0133] (Rust prevention) A CASS test (240 hours) was carried out in accordance with JIS Z 2371:2015, and the rust prevention was evaluated according to the following criteria. - Evaluation criteria - A: Rust width 0.5 mm or less B: Rust width more than 0.5 mm and 1.0 mm or less C: Rust on the entire surface
[0134]
[0135] As shown in Table 8, Examples 2-1 to 2-4 exhibited good adhesion to metal components and good rust prevention properties for the coating film, even when the organic solvent content was 700 g / L or less. On the other hand, Comparative Example 2-1, which did not contain the silane compound (B) having an epoxy group, exhibited poor adhesion and rust prevention. Comparative Example 2-2, which used resin solution P4 that did not contain the nitrogen-containing monomer (a1), exhibited poor adhesion. Comparative Example 2-3, which used resin solution P5 containing 30% by mass of the nitrogen-containing monomer (a1), exhibited poor rust prevention. Comparative Example 2-4, which used resin solution P6 containing an acrylic resin (A) with an acid value of 4 mg KOH / g, exhibited poor adhesion. Comparative Example 2-5, which used resin solution P7 containing an acrylic resin (A) with an acid value of 64 mg KOH / g, exhibited poor rust prevention.
[0136] [Multilayer coating film] Next, using the coating compositions used in Examples 2-1 to 2-4 above as primers, a top coat was formed on the painted bodies of Examples 2-1 to 2-4 above to which the primers had been applied, to form a multilayer coating film, and the multilayer coating film was evaluated.
[0137] [Preparation of Acrylic Resin Solution] First, a resin solution containing an acrylic resin to be used as a top coat paint was prepared. Table 9 shows the components required for preparing the resin.
[0138] [Resin Solution T1] Resin solution T1 containing acrylic resin was prepared according to the following procedure. 30.0 parts by mass of xylene, 31.0 parts by mass of styrene, 12.0 parts by mass of 2-ethylhexyl acrylate, 43.0 parts by mass of 2-ethylhexyl methacrylate, 2.0 parts by mass of acrylic acid, 12 parts by mass of 2-hydroxyethyl methacrylate, and 4.0 parts by mass of 2-2'-azobis-2-methylbutyronitrile were reacted under nitrogen gas at 100°C for 8 hours. The mixture was then diluted with 32.7 parts by mass of xylene to obtain resin solution T1 containing acrylic resin with a heating residue of 60% by mass.
[0139] The acrylic resin contained in the resin solution T1 had a hydroxyl value of 45 mgKOH / g, an acid value of 11 mgKOH / g, a number average molecular weight of 3,500, and a weight average molecular weight of 6,000.
[0140] [Resin Solution T2] Resin solution T2 was prepared in the same manner as resin solution T1, except that the compounds and formulation were changed as shown in Table 9.
[0141] The properties of the acrylic resins of the resulting resin solutions T1 and T2 were evaluated as follows. The evaluation results are shown in Table 9.
[0142] (Heating residue) 1.0 g of the resin solution was precisely weighed into an aluminum cup and dried for 30 minutes in an oven at 150° C. After drying, the mass of the residue was precisely weighed, and the ratio of the mass of the residue to the original mass was calculated as the heating residue (mass %).
[0143] (Hydroxyl value) After the hydroxyl groups in 1 g of acrylic resin were completely acetylated with acetic anhydride, the amount of potassium hydroxide required in mg to neutralize the free acetic acid generated by the acetylation was determined, and this value was taken as the hydroxyl value of the acrylic resin.
[0144] (Acid Value) The acid value of the acrylic resin was determined in accordance with JIS-K-5601-2-1:1999.
[0145] (Number Average Molecular Weight Mn) The number average molecular weight Mn of the acrylic resin was measured using a TSKgel column SuperMultipore HZ-M (manufactured by Tosoh Corporation) by SEC (size exclusion chromatography, product name "HLC-8420GPC", manufactured by Tosoh Corporation) equipped with a differential refractive index (RI) detector. The SEC conditions were tetrahydrofuran as the developing solvent, a flow rate of 0.35 ml / min, and a temperature of 40°C. TSK standard polystyrene (manufactured by Tosoh Corporation) was used as the standard substance.
[0146] (Weight-average molecular weight Mw) The weight-average molecular weight Mw of the acrylic resin was measured using a TSKgel column SuperMultipore HZ-M (manufactured by Tosoh Corporation) by SEC (size exclusion chromatography, product name "HLC-8420GPC", manufactured by Tosoh Corporation) equipped with a differential refractive index (RI) detector. The SEC conditions were tetrahydrofuran as the developing solvent, a flow rate of 0.35 ml / min, and a temperature of 40°C. TSK standard polystyrene (manufactured by Tosoh Corporation) was used as the standard substance.
[0147] (Glass Transition Temperature Tg of Acrylic Resin) The glass transition temperature Tg of the acrylic resin was calculated by Fox's formula.
[0148] (Total Number of Hydroxyl Groups per Number Average Molecular Weight Mn of Acrylic Resin) The total number of hydroxyl groups per number average molecular weight of the acrylic resin was calculated from the measurement result of the number average molecular weight Mn and the value of the hydroxyl value according to the following formula (1): "Total Number of Hydroxyl Groups per Number Average Molecular Weight Mn" = Number Average Molecular Weight of Acrylic Resin × (Hydroxyl Value of Acrylic Resin (mgKOH / g) / 56100) ... (1)
[0149] (Total Number of Hydroxyl Groups per Weight Average Molecular Weight Mw of Acrylic Resin) The total number of hydroxyl groups per weight average molecular weight Mw of the acrylic resin was calculated from the measurement results of the weight average molecular weight Mw and the value of the hydroxyl value according to the following formula (2): "Total number of hydroxyl groups per weight average molecular weight Mw" = Weight average molecular weight of acrylic resin × (Hydroxyl value of acrylic resin (mgKOH / g) / 56100) (2)
[0150]
[0151] [Preparation of Top Coat Paint] Next, top coats were prepared using the resin solutions T1 and T2. The formulations of the components are shown in Table 10.
[0152] [Preparation of Top Coat 1] 61.7 parts by mass of resin solution T1 as the acrylic resin, 26.5 parts by mass of melamine resin solution (a xylene / n-butanol mixed solution of n-butylated melamine resin (heating residue 60% by mass), trade name: AMIDIR L-117-60, manufactured by DIC Corporation) as the crosslinking agent (Y) reactive with hydroxyl groups, 3.0 parts by mass of propylene glycol monomethyl ether acetate, 1.0 part by mass of butyl acetate, and 2.8 parts by mass of Solvesso 150 (manufactured by JX Nippon Oil & Energy Corporation) as the organic solvent (Z), 1.0 part by mass of a hydroxyphenyltriazine-based ultraviolet absorber (trade name: TINUVIN400, manufactured by BASF) as the ultraviolet absorber, and 1.0 part by mass of a hindered amine-based light stabilizer (trade name: EVERSORB93, EVERLIGHT) as the light stabilizer. 1.0 parts by mass of methyl orthoacetate (trade name: MOA, manufactured by Nippoh Chemical Co., Ltd.) was mixed with 3.0 parts by mass of methyl orthoacetate (trade name: MOA, manufactured by Nippoh Chemical Co., Ltd.) as a dehydrating agent, and the mixture was stirred with a disperser to prepare top coat 1.
[0153] [Preparation of Top Coat 2] Top coat 2 was prepared in the same manner as top coat 1, except that the resin solution containing an acrylic resin was changed to resin solution T2.
[0154] (Ford cup viscosity in seconds during application) The flow time of Top Coat 1 and Top Coat 2 during application was measured at 20°C using a Ford cup #4 according to a method in accordance with JIS K5600-2-2:1999.
[0155] [Preparation of topcoat-coated body (substrate: polypropylene)] The above coating composition was spray-coated onto a substrate made of polypropylene, 3.0 mm thick, and 100 mm x 100 mm in size, to a dry film thickness of 30 μm, and then dried at 140° C. for 20 minutes to form a coating film, thereby preparing a coated body (substrate: polypropylene). This coated body was used to measure the glass transition temperature Tg, inter-crosslink molecular weight, and crosslink density of the coating film.
[0156] [Measurement of Top Coat Film Properties (Glass Transition Temperature, Molecular Weight Between Crosslinks, and Crosslink Density)] (Glass Transition Temperature Tg of Coating Film) The coating films of Top Coat 1 and Top Coat 2 were peeled from the polypropylene resin plate and then cut into a sample length of 50 mm and width of 8 mm to prepare measurement samples. The samples were subjected to dynamic viscoelasticity measurement using a dynamic viscoelasticity measuring device RSA G2 (manufactured by TA Instruments) at a measurement length of 24 mm, a frequency of 1 Hz, and a heating rate of 5°C / min. The dynamic glass transition temperature measured as the temperature showing the maximum value of tan δ (loss modulus / storage modulus) was taken as the glass transition temperature.
[0157] (Inter-crosslink molecular weight and crosslink density of coating film) The molecular weight of the resin between crosslinks is called the inter-crosslink molecular weight, and is expressed as the reciprocal of the crosslink density; this value decreases as the crosslink density increases. The inter-crosslink molecular weight of the cured coating film of the present invention is a theoretically calculated value obtained by applying the minimum value of the storage modulus obtained when measuring the glass transition temperature of the cured coating film to the following theoretical formula of rubber viscoelasticity. Formula 1: n = E' / 3RT Where, n: crosslink density (mol / cc) 1 / n: inter-crosslink molecular weight (cc / mol) R: gas constant (8.314 J / K / mol) T: absolute temperature (K) when the storage modulus is E' E': minimum value of the storage modulus (Pa)
[0158]
[0159] Next, the primers of Examples 2-1 to 2-4 and the above-mentioned top coats 1 and 2 were used in the combinations shown in Table 11 to form multilayer coating films.
[0160] [Layer Coating Film Example 1] The coating composition of Example 2-1 was applied as a primer to a substrate made of aluminum, having a thickness of 0.8 mm and a size of 150 mm x 70 mm by air spray coating to a dry film thickness of 25 μm, and the coating composition was then dried for 20 minutes at 140° C. Thereafter, Top Coat 1 was applied to a dry film thickness of 30 μm by air spray coating, and the coated object was then dried for 20 minutes at 140° C. to produce a layered coating film.
[0161] Multilayer Coating Examples 2 to 8 Multilayer coating examples 2 to 8 were prepared in the same manner as multilayer coating example 1, except that the primer and top coat were changed as shown in Table 11.
[0162] [Evaluation of Multilayer Coating Film] The above multilayer coating film examples 1 to 8 were evaluated for adhesion, rust prevention, chemical resistance, coating film hardness, and abrasion resistance. The evaluation methods for adhesion and rust prevention were the same as those described above. Chemical resistance, coating film hardness, and abrasion resistance were evaluated using the following evaluation methods. The evaluation results are shown in Table 11. Note that the evaluations of adhesion and rust prevention in Table 11 are the same as the evaluations of the coating compositions of Examples 2-1 to 2-4, and are reported as primer evaluations.
[0163] (Chemical resistance) 1 ml of an aqueous solution of hydrofluoric acid (10% hydrofluoric acid) was dropped onto the surface of the coating film of each of the above multilayer coating film examples 1 to 8, and then the coating film was left in a test tank without forced convection at a temperature of 23°C for 2 hours for chemical treatment. The aqueous hydrofluoric acid solution was then removed by rinsing with water, and the appearance of the coating film after chemical treatment was visually evaluated according to the following evaluation criteria. - Evaluation criteria - AA: No change in the appearance of the coating film. A: The gloss of the coating film is slightly reduced. C: The gloss of the coating film is significantly reduced.
[0164] (Coating Hardness) The coating hardness of the laminate coating films of the above-mentioned laminate coating film examples 1 to 8 was measured according to "JIS K5600-5-4:1999 Scratch hardness (pencil method)" and evaluated according to the following evaluation criteria. -Evaluation criteria- AA: Pencil hardness is HB or more A: Pencil hardness is 2B or more and B or less C: Pencil hardness is 3B or less
[0165] (Abrasion Resistance) The abrasion resistance of the coating films of the above Multilayer Coating Film Examples 1 to 8 was evaluated as follows. Using a rub fastness tester (manufactured by Daiei Kagaku Seiki Co., Ltd.), a white cloth attached for dye fastness testing in accordance with JIS L 0849 was rubbed back and forth 10 times with a load of 1 kg applied to the surface of the multilayer coating film. After 10 reciprocating strokes, the coating surface was washed with running water and allowed to dry naturally, after which the gloss of the multilayer coating film was visually observed and evaluated according to the following evaluation criteria. - Evaluation Criteria - AA: No change in gloss A: Very slight gloss fade C: Significant gloss fade
[0166]
[0167] As shown in Table 11, the multilayer coating films of Multilayer Coating Film Examples 1 to 8 were evaluated as being good in all of adhesion, rust prevention, chemical resistance, coating hardness and scratch resistance.
[0168] The first coating composition of the present invention can be used as a top coat coating when forming a coating film on a metal substrate in fields such as automobile manufacturing. The second coating composition of the present invention is suitable as a primer coating to be applied to a metal substrate. In particular, it is suitable as a primer coating for aluminum alloy cast wheels of automobiles.
Claims
1. A coating composition comprising an acrylic resin (X) having a total number of hydroxyl groups per number average molecular weight of 2.0 or more and 6.0 or less, a crosslinking agent (Y) that reacts with hydroxyl groups, and an organic solvent (Z), wherein the content of the organic solvent (Z) is 600 g / L or less.
2. The coating composition according to claim 1, wherein the crosslinking agent (Y) which reacts with hydroxyl groups comprises an amino resin.
3. The coating composition according to claim 1, wherein the hydroxyl value calculated from the primary hydroxyl groups of the acrylic resin (X) is from 40 mgKOH / g to 130 mgKOH / g, and the ratio of the primary hydroxyl value to the secondary hydroxyl value is from 100:0 to 100:
60.
4. A coated body having a coating film formed on a substrate from the coating composition according to any one of claims 1 to 3.
5. The coated body according to claim 4, wherein the glass transition temperature Tg of the coating film is 50°C or higher and 98°C or lower.
6. A coating composition comprising: an acrylic resin (A) containing a nitrogen atom-containing monomer (a1) as a polymerizable monomer and having an acid value of 15 mgKOH / g or more and 50 mgKOH / g or less; a silane compound (B) having an epoxy group; and an organic solvent (C), wherein the content of the nitrogen atom-containing monomer (a1) is 5 mass% or more and less than 30 mass% relative to 100 mass% of the total polymerizable monomers; and the content of the organic solvent (C) is 700 g / L or less.
7. The coating composition according to claim 6, wherein the nitrogen atom-containing monomer (a1) is a compound having a functional group capable of reacting with a hydroxyl group.
8. The coating composition according to claim 6, wherein the number average molecular weight of the acrylic resin (A) is 4,000 or more and 10,000 or less.
9. A coating method comprising coating a coating composition according to any one of claims 6 to 8 onto a machined metal substrate.
10. A coated body having a coating film formed from the coating composition according to any one of claims 6 to 8 on a machined metal substrate.
11. The coated body according to claim 10, further comprising a surface protective layer on the coating film.
12. The coated body according to claim 10, further comprising a coating film formed from the coating composition according to claim 1 on said coating film.
Citation Information
Patent Citations
High-solid coating composition
JP2002201430A
Top coat formation method, and clear coating composition used for the same
JP2008126140A
Coating composition and coated body using the same
JP2015067764A
Coating method
JP2019084465A