Prepreg, printed wiring board, and electronic component

The use of a nonwoven fabric-based prepreg with a thermosetting resin in high-speed communication systems addresses the challenge of high dielectric constants in traditional glass cloth prepregs, achieving low dielectric constants and loss tangents, and enabling thinner, more stable printed circuit boards for next-generation communication systems.

WO2024202454A1PCT designated stage expired Publication Date: 2024-10-03MITSUI CHEMICALS INC

Patent Information

Application Number
PCT/JP2024/001897
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-01-23
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Next-generation high-speed communication systems require printed circuit boards with lower dielectric constants and loss tangents to minimize transmission loss, which is challenging with traditional prepregs containing glass cloth due to limitations in fiber diameter and increased manufacturing steps, necessitating a substitute with excellent electrical properties.

Method used

A prepreg comprising a nonwoven fabric with a thermosetting resin, having a dielectric constant of 3.00 or less at 10 GHz, and a nonwoven fabric with an average fiber diameter of 10 μm or less, which eliminates the need for surface treatment and allows for thinner printed circuit boards.

Benefits of technology

The prepreg achieves low dielectric constants and loss tangents, enabling reduced transmission loss and thinner board designs, while simplifying the manufacturing process and improving dimensional stability and fillability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

This prepreg contains a resin-containing nonwoven fabric and a thermosetting resin, and has a dielectric constant of 3.00 or less at 10 GHz.
Need to check novelty before this filing date? Find Prior Art

Description

Prepreg, printed wiring boards and electronic components

[0001] The present disclosure relates to a prepreg, a printed wiring board, and an electronic component.

[0002] Next-generation high-speed communications are expected to evolve significantly compared to previous communication systems, with features such as higher speed, larger capacity, lower latency, and multiple connections. Furthermore, higher frequency ranges will be used in next-generation high-speed communications, and printed circuit boards will be required to achieve higher speeds and larger capacities (for example, thinner board components), lower latency, and lower transmission loss. Since transmission loss is proportional to frequency, the square root of the relative permittivity, and the dielectric loss tangent, low permittivity and low dielectric loss tangent are required in the high-frequency band.

[0003] As a prepreg contained in a printed circuit board, a prepreg containing a glass cloth and a matrix resin is generally known. Furthermore, Patent Document 1 proposes a glass cloth for a low dielectric material, the surface of which is treated with a polysilazane-containing composition. [Patent Document 1] JP 2020-194888 A

[0004] Prepregs containing glass cloth generally have higher dielectric constants, dielectric loss tangents, etc. than matrix resins. Therefore, from the viewpoint of reducing transmission loss, it is desirable to improve the dielectric properties by surface treating the glass cloth, as disclosed in Patent Document 1.

[0005] As shown in Patent Document 1, when glass cloth is used, surface treatment of the glass cloth is required to improve electrical properties, which increases the number of steps. Furthermore, there are restrictions on how thin the fiber diameter of glass cloth can be made due to legal regulations and other reasons, which limits how thin the printed circuit board can be made. Considering the simplification of the prepreg production process and further thinning of printed circuit boards, a prepreg with excellent electrical properties such as a low dielectric constant and a low dielectric loss tangent is desirable as an alternative to prepregs containing surface-treated glass cloth.

[0006] An object of one aspect of the present disclosure is to provide a prepreg that is an alternative to a prepreg containing glass cloth and has excellent electrical properties, as well as a printed wiring board and an electronic component that include a cured product of this prepreg.

[0007] Means for solving the above problems include the following aspects. <1> A prepreg comprising a resin-containing nonwoven fabric and a thermosetting resin, having a dielectric constant of 3.00 or less at 10 GHz. <2> The prepreg according to <1>, wherein the nonwoven fabric has an average fiber diameter of 10 μm or less. <3> The prepreg according to <1>, wherein the nonwoven fabric has an average fiber diameter of 3 μm or less. <4> The prepreg according to <1>, wherein the nonwoven fabric has an average fiber diameter of 0.5 μm to 1.8 μm. <5> The prepreg according to any one of <1> to <4>, wherein the nonwoven fabric contains a thermoplastic resin. <6> The prepreg according to <5>, wherein the thermoplastic resin has a melting point of 200°C or higher. <7> The prepreg according to <5> or <6>, wherein the thermoplastic resin contains syndiotactic polystyrene. <8> The prepreg according to any one of <1> to <7>, wherein the thermosetting resin comprises at least one selected from the group consisting of epoxy resin, melamine resin, phenolic resin, unsaturated polyester resin, and silicone resin. <9> The prepreg according to any one of <1> to <8>, wherein the proportion of the nonwoven fabric is 20% by mass to 80% by mass based on the total amount of the prepreg. <10> The prepreg according to any one of <1> to <9>, wherein the dielectric dissipation factor at 10 GHz of the prepreg is 0.0050 or less. <11> The prepreg according to any one of <1> to <10>, wherein the dimensional change rate of the prepreg before and after curing is 5% or less. <12> A printed wiring board comprising a cured product of the prepreg according to any one of <1> to <11>. <13> An electronic component comprising an insulating layer comprising a cured product of the prepreg according to any one of <1> to <11>.

[0008] According to one aspect of the present disclosure, there is provided a prepreg that is an alternative to a prepreg containing glass cloth and has excellent electrical properties, as well as a printed wiring board and an electronic component that include a cured product of this prepreg.

[0009] In this disclosure, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. In this disclosure, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. In this disclosure, when multiple substances corresponding to each component are present in the composition, the amount of each component contained in the composition means the total amount of the multiple substances present in the composition, unless otherwise specified. In the numerical ranges described in stages in this disclosure, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Furthermore, in the numerical ranges described in this disclosure, the upper or lower limit of that numerical range may be replaced with a value shown in the examples.

[0010] [Prepreg] The prepreg of the present disclosure comprises a resin-containing nonwoven fabric and a thermosetting resin, and has a dielectric constant of 3.00 or less at 10 GHz. The prepreg of the present disclosure is a prepreg with excellent electrical properties, such as a low dielectric constant and a low dielectric loss tangent. Furthermore, since a resin-containing nonwoven fabric is used instead of glass cloth, the prepreg has excellent electrical properties even without surface treatment or the like aimed at achieving a low dielectric constant. Furthermore, by adjusting the manufacturing method and manufacturing conditions of the nonwoven fabric, the fiber diameter can be reduced, and printed circuit boards and the like using the prepreg can also be made thinner.

[0011] The dielectric constant (relative permittivity) of the prepreg at 10 GHz is 3.00 or less, more preferably 2.90 or less, and even more preferably 2.80 or less. The lower limit of the dielectric constant of the prepreg at 10 GHz is not particularly limited, and may be, for example, 2.00 or more, 2.30 or more, or 2.50 or more.

[0012] The dielectric loss tangent of the prepreg at 10 GHz is preferably 0.0050 or less, more preferably 0.0045 or less, and even more preferably 0.0040 or less. The lower limit of the dielectric loss tangent of the prepreg at 10 GHz is not particularly limited, and may be, for example, 0.0010 or more, 0.0020 or more, or 0.0025 or more.

[0013] The dielectric constant and dielectric loss tangent of a prepreg at 10 GHz can be determined by the following method. First, a 10 cm x 10 cm test piece is prepared using a cured prepreg. The dielectric constant (relative permittivity) and dielectric loss tangent of the obtained test piece at 10 GHz are measured using a cavity resonator dielectric constant measuring device (for example, manufactured by Kanto Electronics Application Development Co., Ltd.).

[0014] The dimensional change rate of the prepreg before and after curing is preferably 15% or less, more preferably 10% or less, and even more preferably 5% or less. The dimensional change rate of the prepreg before and after curing is calculated from the dimension SB of the prepreg before curing and the dimension SA of the prepreg after curing according to the following formula: Dimensional change rate (%) (= [SB / SA] × 100) The lower limit of the dimensional change rate of the prepreg before and after curing may be 0% or more.

[0015] (Nonwoven Fabric) The prepreg of the present disclosure includes a resin-containing nonwoven fabric. From the viewpoint of reducing the thickness when the prepreg is applied to a printed wiring board, electronic component, etc., the nonwoven fabric preferably has an average fiber diameter of 10 μm or less, more preferably 3 μm or less, even more preferably 0.1 μm to 2.0 μm, and particularly preferably 0.5 μm to 1.8 μm.

[0016] The average fiber diameter of a nonwoven fabric can be determined as follows: A photograph of the surface of the nonwoven fabric to be measured is taken at 1000x magnification using an electron microscope (model number: S-3500N, manufactured by Hitachi, Ltd.). From the photograph, 100 fibers (n=100) are randomly selected, the diameters (widths) of the selected fibers are measured, and the arithmetic mean value is determined as the average fiber diameter (Da).

[0017] The type of nonwoven fabric is not particularly limited, and examples thereof include various nonwoven fabrics such as meltblown nonwoven fabrics, spunbond nonwoven fabrics, carded air-through nonwoven fabrics, airlaid nonwoven fabrics, needle-punched spunbond nonwoven fabrics, wet-laid nonwoven fabrics, dry-laid pulp nonwoven fabrics, flash-spun nonwoven fabrics, and spread-fiber nonwoven fabrics. Among these, meltblown nonwoven fabrics are preferred from the viewpoint of reducing the fiber diameter. The nonwoven fabric may be either a long-fiber nonwoven fabric or a short-fiber nonwoven fabric.

[0018] The nonwoven fabric preferably contains a thermoplastic resin as the resin. The thermoplastic resin contained in the nonwoven fabric may be one type alone or two or more types in combination.

[0019] When the nonwoven fabric contains a thermoplastic resin, the content of the thermoplastic resin is preferably 70% by mass to 100% by mass, more preferably 90% by mass to 100% by mass, even more preferably 95% by mass to 100% by mass, and particularly preferably 99% by mass to 100% by mass, based on the total amount of resin.

[0020] The melting point of the thermoplastic resin is preferably 200°C or higher from the viewpoint of suppressing voids in the prepreg, and more preferably 240°C or higher, further preferably 260°C or higher, and particularly preferably 270°C or higher from the viewpoint of dimensional stability before and after curing of the prepreg and filling properties during prepreg production. The upper limit of the melting point of the thermoplastic resin is not particularly limited, and may be, for example, 300°C or lower, or 280°C or lower.

[0021] The melting point of a nonwoven fabric can be determined as follows: Using 10 mg of nonwoven fabric as a sample, (i) heat the sample to 300°C at 20°C / min and hold it at 300°C for 5 minutes, (ii) cool the sample to 40°C at 20°C / min and hold it at 40°C for 1 minute, and then (iii) heat the sample to 300°C at 20°C / min. The highest endothermic peak temperature among the endothermic peak temperatures observed in the differential scanning calorimetry curve (DSC curve) during the second heating process (iii) is determined to be the melting point of the nonwoven fabric.

[0022] The thermoplastic resin is not particularly limited, and examples thereof include polyolefin, polyamide, polyacetal, polycarbonate, modified polyphenylene ether, polybutylene terephthalate, polyethylene terephthalate, syndiotactic polystyrene, atactic polystyrene, isotactic polystyrene, cyclic polyolefin, polyphenylene sulfide, polytetrafluoroethylene, perfluoroalkoxyalkane, ethylene tetrafluoroethylene, polysulfone, polyethersulfone, amorphous polyarylate, polyetheretherketone, thermoplastic polyimide, polyamideimide, and copolymers thereof. Among these, from the viewpoints of heat resistance and electrical properties, it is preferable that the thermoplastic resin contains syndiotactic polystyrene.

[0023] The thermoplastic resins used in the present disclosure, for example, the thermoplastic resins exemplified above such as polyolefin and syndiotactic polystyrene, may be resins derived from biomass or resins derived from fossil resources.

[0024] When the thermoplastic resin contains syndiotactic polystyrene, the content of syndiotactic polystyrene is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and even more preferably 90% by mass to 100% by mass, based on the total amount of the thermoplastic resin.

[0025] The content of syndiotactic polystyrene in the nonwoven fabric is preferably 7% by mass to 100% by mass, more preferably 90% by mass to 100% by mass, even more preferably 95% by mass to 100% by mass, and particularly preferably 99% by mass to 100% by mass, based on the total amount of the nonwoven fabric.

[0026] The melt flow rate (MFR) of the thermoplastic resin (preferably, syndiotactic polystyrene) at 300°C under a load of 1.2 kg is preferably 50 g / 10 min to 100 g / 10 min, more preferably 55 g / 10 min to 90 g / 10 min, and even more preferably 60 g / 10 min to 80 g / 10 min. When the MFR of the thermoplastic resin (preferably, syndiotactic polystyrene) at 300°C under a load of 1.2 kg is 50 g / 10 min or more, this tends to enable the average fiber diameter to be made thinner, which is preferable. When the MFR is 100 g / 10 min or less, this tends to improve the strength of the fiber and inhibit the generation of decomposition components, which is preferable.

[0027] MFR is measured in accordance with ASTM D-1238 (Method B) under the following conditions. The measurement sample is pre-dried at 120°C for 6 hours before measurement. Test method: ASTM D1238 (Method B) Filling amount: 8.0 g Test temperature: 300°C Load: 1.2 kg Measurement is performed three times under the above conditions, and the average value is calculated. As a measuring device, for example, a Melt Indexer F-F01 type (Toyo Seiki Seisakusho, Ltd.) can be used.

[0028] The dielectric constant (relative permittivity) of the nonwoven fabric at 10 GHz is preferably 3.00 or less, more preferably 2.50 or less, and even more preferably 2.40 or less. The lower limit of the dielectric constant of the nonwoven fabric at 10 GHz is not particularly limited, and may be, for example, 1.50 or more, 2.00 or more, or 2.20 or more.

[0029] The dielectric loss tangent of the nonwoven fabric at 10 GHz is preferably 0.001 or less, more preferably 0.0008 or less, and even more preferably 0.0006 or less. The lower limit of the dielectric loss tangent of the nonwoven fabric at 10 GHz is not particularly limited, and may be, for example, 0.0001 or more, 0.0002 or more, or 0.0004 or more.

[0030] The dielectric constant and dielectric loss tangent of the nonwoven fabric at 10 GHz can be determined in the same manner as the dielectric constant and dielectric loss tangent of the prepreg at 10 GHz described above.

[0031] The basis weight of the nonwoven fabric is not particularly limited and can be determined appropriately depending on the application. For example, the basis weight of the nonwoven fabric is 0.5 g / cm 2 ~200g / m 2 It is preferable that the density is 1 g / m 2 ~100g / m 2 More preferably, it is 1 g / m 2 ~30g / m 2 It is more preferable that:

[0032] The basis weight of a nonwoven fabric can be determined as follows. Ten test pieces of 100 mm (fiber flow direction: MD) x 100 mm (direction perpendicular to the fiber flow direction (CD direction)) are taken from the nonwoven fabric. The test pieces are taken from 10 locations in the CD direction. Next, a top-pan electronic balance (manufactured by Kensei Kogyo Co., Ltd.) is used to measure the mass [g] of each of the test pieces taken, and the average mass of each test piece is determined. The average mass of each test piece is then calculated by subtracting 1 m from the average value determined above. 2 The weight per unit area of ​​each nonwoven fabric was calculated as [g / m 2 〕

[0033] There are no particular limitations on the method for adjusting the basis weight of the nonwoven fabric to the above range, and examples thereof include a method of adjusting the speed of a collector during the production of the nonwoven fabric.

[0034] The thickness of the nonwoven fabric is not particularly limited and can be determined appropriately depending on the application. For example, the thickness of the nonwoven fabric is preferably 5 μm to 10 mm, more preferably 6 μm to 1 mm, and even more preferably 8 μm to 500 μm.

[0035] The thickness of the nonwoven fabric can be determined as follows. For 10 sheets of nonwoven fabric to be measured, the thickness was measured at five locations, namely the center and four corners, and the average value of the 10 locations was calculated. The thickness was measured under a load of 7 gf / cm. 2 A thickness gauge (measuring probe diameter 50 mm) was used.

[0036] The proportion of the nonwoven fabric is preferably 20% by mass to 80% by mass, more preferably 25% by mass to 75% by mass, and even more preferably 30% by mass to 70% by mass, based on the total amount of the prepreg.

[0037] The nonwoven fabric may contain, as necessary, various known additives such as antioxidants, heat stabilizers, weather stabilizers, antistatic agents, slip agents, antifogging agents, lubricants, dyes, pigments, natural oils, synthetic oils, waxes, fatty acid amides, etc. When the prepreg of the present disclosure is used for printed wiring boards, electronic components, etc., from the viewpoint of long-term reliability of the circuit boards, etc., the content of these additives in the nonwoven fabric is preferably low, specifically, preferably 0.1 mass% or less, more preferably 0.05 mass% or less, and even more preferably 0.01 mass% or less.

[0038] (Thermosetting Resin) The prepreg of the present disclosure includes a thermosetting resin.

[0039] Examples of thermosetting resins include epoxy resins, melamine resins, phenolic resins, unsaturated polyester resins, and silicone resins. Among the above, the thermosetting resin preferably includes an epoxy resin. The thermosetting resin may be a single type or a combination of two or more types. The thermosetting resin used in the present disclosure, for example, the thermosetting resins exemplified above such as epoxy resins, may be a resin derived from biomass or a resin derived from fossil resources.

[0040] (Other Components) The prepreg of the present disclosure may contain components other than the nonwoven fabric and thermosetting resin described above. The prepreg may contain various known additives, such as fillers, antioxidants, heat stabilizers, weather stabilizers, antistatic agents, slip agents, antifogging agents, lubricants, dyes, pigments, natural oils, synthetic oils, waxes, and fatty acid amides, as needed. The content of these additives in the prepreg may be 30% by mass or less, 20% by mass or less, 10% by mass or less, or 1% by mass or less, based on the total amount of the prepreg.

[0041] The thickness of the prepreg can be appropriately selected depending on the intended use. It can also be adjusted by the thickness of the nonwoven fabric, the type of resin constituting the nonwoven fabric, the impregnation time of the resin composition, the amount of the resin composition used for impregnation, etc. The thickness of the prepreg is preferably 10 μm to 10 mm, more preferably 20 μm to 1 mm, and even more preferably 30 μm to 500 μm, from the viewpoint of improving, for example, the shapeability when laminating the prepreg and the mechanical strength and toughness of the cured product.

[0042] The use of the prepreg of the present disclosure is not particularly limited, and it can be used, for example, in printed wiring boards, conductor laminates, electronic components, etc., which will be described later.

[0043] The method for producing the prepreg is not particularly limited, and known production methods can be applied. For example, a method for producing the prepreg includes a step of impregnating a nonwoven fabric with a varnish containing a resin composition to obtain an impregnated body, and a step of heating the obtained impregnated body to remove the solvent contained in the varnish and drying it. Impregnation of the nonwoven fabric with the varnish containing the resin composition can be carried out by applying a predetermined amount of varnish to the nonwoven fabric by a known method such as spray coating, dip coating, roll coating, curtain coating, die coating, or slit coating, and then, if necessary, placing a protective film on top of the varnish and pressing it from above with a roller or the like. The method for heating the impregnated body to dry the solvent contained in the varnish is not particularly limited, and examples thereof include a batch method of drying the impregnated body in an air or nitrogen atmosphere using a blower dryer, and a continuous method of drying the impregnated body through a heating furnace.

[0044] [Conductor clad laminate] The conductor clad laminate of the present disclosure is a laminate in which a conductor layer is laminated on at least one surface of the prepreg of the present disclosure. The conductor clad laminate of the present disclosure has the above-mentioned configuration and therefore has excellent electrical properties. The conductor layer is not particularly limited as long as it is a layer containing a conductive material, and examples thereof include metal foils. Examples of metal foils include copper foil, aluminum foil, nickel foil, gold foil, silver foil, and stainless steel foil. The metal clad laminate of the present disclosure can be manufactured by known manufacturing methods.

[0045] [Printed Wiring Board] The printed wiring board of the present disclosure is a printed wiring board including a cured product of the prepreg of the present disclosure. The printed wiring board of the present disclosure has the above-described configuration and therefore has excellent electrical properties.

[0046] More specifically, the printed wiring board preferably comprises a cured prepreg and a conductor layer with wiring formed on one or both sides of the cured prepreg.

[0047] The printed wiring board may be provided with a conductor layer having an antenna circuit formed on one or both sides of the cured prepreg of the present disclosure.

[0048] The method for producing a printed wiring board is not particularly limited, and known production methods can be applied. For example, in a method for producing a printed wiring board, the prepreg produced by the above-mentioned method is heat-cured using a lamination press or the like to form an insulating layer. Next, a conductor layer is laminated on the obtained insulating layer using a known method to produce a laminate. Thereafter, the conductor layer in the laminate is subjected to circuit processing or the like to obtain a printed wiring board.

[0049] The conductor layer is preferably a metal layer containing a metal. Examples of metals include copper, aluminum, nickel, gold, silver, and stainless steel. Methods for forming the conductor layer include, for example, a method in which a conductive material such as a metal is made into a foil and heat-sealed to an insulating layer; a method in which an insulating layer and a conductor layer are bonded using an adhesive; and a method in which a conductor layer is formed by sputtering, vapor deposition, plating, or the like. The printed wiring board may be either a single-sided board or a double-sided board. The printed wiring board of the present disclosure can be used as an electronic component by mounting electronic components such as semiconductor elements thereon.

[0050] [Electronic Component] The electronic component of the present disclosure is an electronic component having an insulating layer containing a cured product of the prepreg of the present disclosure. Because the electronic component of the present disclosure has the above-described configuration, it has excellent electrical properties. The method for manufacturing the electronic circuit is not particularly limited, and known manufacturing methods can be applied.

[0051] The electronic component of the present disclosure may be an electronic component having a circuit for transmitting an electric signal of 1 GHz or more, such as a high-frequency antenna circuit, a backplane of a high-speed server or router, or a high-speed transmission flexible substrate used in a hard disk, a liquid crystal display, or the like.

[0052] Examples of the present disclosure will be described below, but the present disclosure is not limited to the following examples.

[0053] Example 1 (Preparation of Nonwoven Fabric) Syndiotactic polystyrene (SPS in Table 1, MFR: 60 g / 10 min at 300°C and a load of 1.2 kg) was fed into a single-screw kneading extruder through a hopper and melt-kneaded at 340°C. The melt-kneaded material was then mixed with heated air (340°C, 770 Nm) blown from both sides of a nozzle. 3 The conditions for this were a spinning temperature of 340°C, a nozzle die with a hole diameter of 0.20 mm, and a single hole discharge rate of 0.10 g / min. The discharged fibrous material was then collected in the form of a web to obtain a meltblown nonwoven fabric with the physical properties shown in Table 1.

[0054] (Preparation of Prepreg) A thermosetting resin, bisphenol A epoxy resin (trade name JER828, manufactured by Mitsubishi Chemical Corporation) and 1-benzyl-2-phenylimidazole (Curesol 1B2PZ, manufactured by Shikoku Chemical Industry Co., Ltd.) were dissolved in a toluene solvent to obtain a resin varnish. A meltblown nonwoven fabric was then impregnated with this resin varnish and dried in an air dryer to obtain a cured prepreg having a thickness of 40 μm.

[0055] [Examples 2 and 3] Meltblown nonwoven fabrics were produced in the same manner as in Example 1, except that the production conditions for the nonwoven fabric were changed so that the basis weight and thickness would be as shown in Table 1. Then, cured prepregs having a thickness of 65 μm or 130 μm were obtained using the same procedure as in Example 1.

[0056] [Example 4] Polymethylpentene (TPX: registered trademark in Table 1) was fed into a single-screw kneading extruder through a hopper and melt-kneaded at 330°C. The melt-kneaded material was then mixed with heated air (330°C, 690 Nm) blown from both sides of the nozzle. 3 / h / m), and extruded in a fibrous form. The conditions were a spinning temperature of 330°C, a nozzle die with a hole diameter of 0.20 mmφ, and a single-hole extrusion rate of 0.11 g / min. The extruded fibrous material was then collected in a web form to obtain a meltblown nonwoven fabric with the physical properties shown in Table 1. A cured prepreg having a thickness of 140 μm was obtained by the same procedure as in Example 1, except that the meltblown nonwoven fabric produced in Example 4 was used.

[0057] [Example 5] Propylene homopolymer (PP in Table 1) was fed into a single-screw kneading extruder through a hopper and melt-kneaded at 290°C. The melt-kneaded material was then mixed with heated air (290°C, 610 Nm) blown from both sides of the nozzle. 3 The material was extruded in a fibrous form together with the cellulose acylate / h / m. The conditions were a spinning temperature of 290°C, a nozzle die with a hole diameter of 0.20 mmφ, and a single-hole extrusion rate of 0.12 g / min. The extruded fibrous material was then collected in a web form to obtain a meltblown nonwoven fabric with the physical properties shown in Table 1. A cured prepreg having a thickness of 160 μm was obtained in the same manner as in Example 1, except that the meltblown nonwoven fabric produced in Example 5 was used.

[0058] Comparative Example 1 A glass cloth (glass cloth for printed wiring boards, IPC Spec 1017, manufactured by Nitto Boseki Co., Ltd.) was prepared. A cured prepreg having a thickness of 90 μm was obtained in the same manner as in Example 1, except that the glass cloth was used instead of the nonwoven fabric.

[0059] (Preparation of Copper-Clad Laminates) In each of the Examples and Comparative Examples, eight prepregs cut into 150 mm squares were stacked, and copper foil (F1-WS, manufactured by Furukawa Electric Co., Ltd.) was then stacked on both ends in the stacking direction. Next, the stack was heated in a vacuum press at a pressure of 3.5 MPa and 200°C for 2 hours to prepare copper-clad laminates with the copper foil adhered thereto.

[0060] The physical properties of the nonwoven fabric (meltblown nonwoven fabric) and glass cloth used in each example and comparative example are as shown in Table 1. The term "body" in Table 1 refers to the nonwoven fabric or glass cloth. For each example and comparative example, the methods for measuring the physical properties and the methods for evaluating the prepregs are shown below, and the measurement results and evaluation results are shown in Table 1.

[0061] -Method for measuring dielectric constant and dielectric loss tangent- Test specimens measuring 10 cm x 10 cm were prepared using the cured prepregs prepared in each Example and Comparative Example. The dielectric constant (relative dielectric constant) and dielectric loss tangent at 10 GHz of the obtained test specimens were measured using a cavity resonator dielectric constant measuring device (manufactured by Kanto Electronics Application Development Co., Ltd.). The dielectric constant (relative dielectric constant) and dielectric loss tangent at 10 GHz of the nonwoven fabric and glass cloth were also measured using the same method.

[0062] -Evaluation of Electrical Properties- Based on the results of the dielectric constant and dielectric dissipation factor at 10 GHz in each of the Examples and Comparative Examples, the electrical properties were evaluated according to the following criteria: <Evaluation criteria> A: Dielectric constant at 10 GHz is 3.00 or less, and dielectric dissipation factor is 0.0030 or less B: Dielectric constant at 10 GHz is greater than 3.00, and dielectric dissipation factor is greater than 0.0030

[0063] - Evaluation - (1) Dimensional Stability The dimensions of the prepreg before and after curing, that is, the dimension SB of the nonwoven fabric of each example that was impregnated with resin varnish and contained the resin varnish in an uncured state during the production of the prepreg, was compared with the dimension SA of the prepreg after curing, to determine the dimensional change rate (%) (= [SB / SA] x 100). The dimensional change rate was evaluated according to the following evaluation criteria. <Evaluation Criteria> G1: The dimensional change rate was 5% or less. G2: The dimensional change rate was more than 5% but not more than 15%. G3: The dimensional change rate was more than 15%.

[0064] (2) Filling Ability When producing the prepreg, the time required for the resin varnish to be impregnated into the nonwoven fabric was measured, and the filling ability was evaluated according to the following evaluation criteria. The time required for impregnation is the time required from the time the nonwoven fabric is impregnated with the resin varnish until there are no more visually visible unimpregnated areas or bubbles. G1: Less than 1 minute. G2: 1 minute or more but less than 5 minutes. G3: 5 minutes or more, or impregnation was not complete naturally.

[0065] (3) Voids The copper clad laminate was cut in the thickness direction, and the cut surface was imaged at 10 locations using a scanning electron microscope at 1000x magnification, and the presence or absence of voids was evaluated according to the following criteria: G1: No voids were observed on the observed surface, G2: One void was observed on the observed surface, G3: 10 or more voids were observed on the observed surface.

[0066]

[0067] As shown in Table 1, the prepregs produced in Examples 1 to 5 had better electrical properties than the prepreg produced in Comparative Example 1. Because a lower dielectric constant and a lower dielectric loss tangent were possible compared to Comparative Example 1, they were superior in terms of shortening delay time and reducing transmission loss. Furthermore, the prepregs produced in Examples 1 to 3 were evaluated as being good in terms of dimensional stability, filling ability, and voids. From the above points, it is presumed that the prepregs of the present disclosure are useful for communication technologies that require high-speed, large-capacity communication, low latency, an increased number of simultaneous connections, etc.

[0068] The disclosure of Japanese Patent Application No. 2023-049053, filed on March 24, 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards mentioned herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.

Claims

1. A prepreg comprising a resin-containing nonwoven fabric and a thermosetting resin, and having a dielectric constant of 3.00 or less at 10 GHz.

2. The prepreg according to claim 1, wherein the average fiber diameter of the nonwoven fabric is 10 μm or less.

3. The prepreg according to claim 1, wherein the average fiber diameter of the nonwoven fabric is 3 μm or less.

4. The prepreg according to claim 1, wherein the average fiber diameter of the nonwoven fabric is 0.5 μm to 1.8 μm.

5. The prepreg according to claim 1, wherein the nonwoven fabric comprises a thermoplastic resin.

6. The prepreg according to claim 5, wherein the melting point of the thermoplastic resin is 200°C or higher.

7. The prepreg according to claim 5, wherein the thermoplastic resin comprises syndiotactic polystyrene.

8. The prepreg according to claim 1, wherein the thermosetting resin comprises at least one selected from the group consisting of epoxy resin, melamine resin, phenolic resin, unsaturated polyester resin and silicone resin.

9. The prepreg according to claim 1, wherein the proportion of said nonwoven fabric is 20% by mass to 80% by mass based on the total amount of the prepreg.

10. The prepreg according to claim 1, wherein the prepreg has a dielectric tangent at 10 GHz of 0.0050 or less.

11. The prepreg according to claim 1, in which the dimensional change rate of the prepreg before and after curing is 5% or less.

12. A printed wiring board comprising a cured product of the prepreg according to any one of claims 1 to 11.

13. An electronic component comprising an insulating layer containing a cured product of the prepreg according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Method for preparing embedded material and embedded material prepared thereby

    CN101973145A

  • Nonwoven fabric for electronic component and laminate for the same

    JP2000260229A

  • Resin laminate plate for printed wiring board

    JP2002064254A

  • Fibers made from syndiotactic vinyl aromatic polymers having long-chain branching.

    JP2002508811A

  • Resin composition having low dielectric loss tangent, cured product of the same, prepreg using the same composition, laminated plate and multilayered printed board

    JP2003012710A

Cited By

  • Wet-laid nonwoven fabrics and their manufacturing methods, as well as prepregs and metal-clad laminates.

    JP2026142959A