Active energy ray-curable ink, method for producing same, and printed matter

Active energy ray-curable inks with a (meth)acryloyl group concentration of 4.0 to 8.0 mmol/g, formulated using specific reactants, address curability and printability issues, resulting in reduced ink mist and bottle escape, and improved curability and productivity.

WO2024202482A1PCT designated stage expired Publication Date: 2024-10-03TOYO INK MFG CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/002444
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-01-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Active energy ray-curable inks face challenges with ink curability and printability due to low (meth)acryloyl group concentrations in binder resins, leading to ink mist and bottle escape issues during printing, and require improved (meth)acryloyl group introduction to enhance productivity and curability.

Method used

Formulating active energy ray-curable inks with urethane (meth)acrylate having a (meth)acryloyl group concentration between 4.0 to 8.0 mmol/g, using specific (meth)acrylic compounds, polyol compounds, and isocyanate compounds to achieve improved printability and curability, and producing the ink through a method involving the reaction of these components.

Benefits of technology

The ink exhibits enhanced printability and curability, reducing ink mist and bottle escape issues, while maintaining excellent curability and productivity, as demonstrated by evaluations showing improved performance in ink mist and moist heat blocking tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided is an active energy ray-curable ink containing a urethane (meth)acrylate (A) and a (meth)acrylic compound (B) other than (A), wherein the (meth)acryloyl group concentration of the urethane (meth)acrylate (A) is in the range of 4.0-8.0 mmol / g.
Need to check novelty before this filing date? Find Prior Art

Description

Active energy ray curable ink, its manufacturing method, and printed matter

[0001] An embodiment of the present invention relates to an actinic radiation-curable ink, a method for producing the same, and a printed matter.

[0002] In recent years, there has been an increasing demand for shorter printing turnaround times and environmental friendliness. In response to these demands, the use of fast-drying, solvent-free active energy ray-curable inks has expanded in place of conventional oil-based inks. Active energy ray-curable inks contain, as a constituent, an active energy ray-curable unsaturated compound, such as an acrylic ester compound. Active energy ray-curable inks containing such unsaturated compounds instantly cure upon exposure to active energy rays, forming a tough film due to three-dimensional crosslinking of the unsaturated compound. Furthermore, because such active energy ray-curable inks instantly cure, post-processing can be performed immediately after printing. For this reason, active energy ray-curable inks are favorably used in packaging printing and commercial form printing, where a strong film is required for improved productivity and design protection.

[0003] In active energy ray-curable inks (hereinafter sometimes referred to as "inks"), binder resins, such as diallyl phthalate resins, are often used to impart printability. However, because most binder resins do not contain (meth)acryloyl groups, the binder resins do not participate in the formation of three-dimensional crosslinks in the cured film of the active energy ray-curable ink, resulting in a problem of degraded ink curability. On the other hand, the use of urethane acrylate, a binder resin containing (meth)acryloyl groups, can solve the problem of ink curability.

[0004] For example, Patent Document 1 discloses an ink using a urethane acrylate made from hydroxyethyl acrylate, polyol, and polymeric MDI, with a (meth)acryloyl group concentration ranging from 1.5 to 3.9 mmol / g. Patent Document 2 discloses an ink using a urethane acrylate made from pentaerythritol triacrylate, polypropylene glycol with a molecular weight of 1000, and isophorone diisocyanate. However, the (meth)acryloyl group concentration of the urethane acrylate in Patent Document 2 is only approximately 1.6 mmol / g. Further improvements in productivity and reductions in the amount of active energy radiation exposure are required in printing sites. Therefore, there is a need to improve the curing properties of inks by further introducing (meth)acryloyl groups into the urethane acrylate.

[0005] Furthermore, compared to oil-based inks, active energy ray-curable inks are prone to problems such as ink mist being generated by the rotation of the rollers inside the printing press, causing the printing press to become dirty, and poor ink fluidity, which means that the ink is prone to being unable to be scraped off from the ink fountain by the rollers during printing (ink fountain run-off).

[0006] International Publication No. 2016 / 63625 Japanese Patent Application Laid-Open No. 60-161468

[0007] The present invention provides an actinic ray-curable ink having improved printability and curability, and also provides a printed matter using the ink.

[0008] The present inventors discovered that an active energy ray-curable ink containing a urethane (meth)acrylate having a (meth)acryloyl group concentration in the range of 4.0 to 8.0 mmol / g eliminates problems of ink mist and ink runoff during printing and provides an ink with excellent curing properties, leading to the completion of the present invention. Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the embodiments described below and various modifications are possible.

[0009] <1> An active energy ray-curable ink containing a urethane (meth)acrylate (A) and a (meth)acrylic compound (B) other than the (A), wherein the (meth)acryloyl group concentration of the urethane (meth)acrylate (A) is in the range of 4.0 to 8.0 mmol / g.

[0010] <2> The active energy ray-curable ink according to the above <1>, wherein the urethane (meth)acrylate (A) is a reaction product of a (meth)acrylic compound (a1) having one or more hydroxyl groups, a polyol compound (a2) other than (a1), and an isocyanate compound (a3).

[0011] <3> The active energy ray-curable ink according to the above <2>, wherein the (meth)acrylic compound (a1) having one or more hydroxyl groups includes at least one compound selected from the group consisting of pentaerythritol poly(meth)acrylate, dipentaerythritol poly(meth)acrylate, and polypentaerythritol poly(meth)acrylate.

[0012] <4> The actinic ray-curable ink according to the above item <2> or <3>, wherein the polyol compound (a2) includes at least one selected from the group consisting of polyol compounds having 3 to 20 carbon atoms and alkylene oxide-modified polyol compounds having 3 to 20 carbon atoms.

[0013] <5> The actinic ray-curable ink according to any one of the above <2> to <4>, wherein the polyol compound (a2) is at least one selected from the group consisting of propylene glycol, butanediol, neopentyl glycol, hexanediol, octanediol, decanediol, glycerin, trimethylolpropane, pentaerythritol, and alkylene oxide-modified products thereof.

[0014] <6> The actinic ray-curable ink according to any one of the above <2> to <5>, wherein the polyol compound (a2) has a hydroxyl value of 125 to 1850 mgKOH / g.

[0015] <7> The active energy ray-curable ink according to any one of the above <2> to <6>, wherein the isocyanate compound (a3) ​​is a diisocyanate compound.

[0016] <8> The active energy ray-curable ink according to any one of the above <2> to <7>, wherein the ratio [(a1') / (a3')] of the number of moles (a1') of hydroxyl groups contained in the (meth)acrylic compound (a1) having one or more hydroxyl groups to the number of moles (a3') of isocyanate groups contained in the isocyanate compound (a3) ​​is in the range of 0.2 to 0.6.

[0017] <9> A method for producing the active energy ray-curable ink according to any one of the above items <1> to <8>, comprising the step of reacting a (meth)acrylic compound (a1) having one or more hydroxyl groups, a polyol compound (a2) other than the (a1), and an isocyanate compound (a3) ​​in a (meth)acrylic compound (B) to obtain the urethane (meth)acrylate (A).

[0018] <10> A printed material having, on a substrate, a cured product of the actinic ray-curable ink according to any one of <1> to <8> above. The disclosure of the present application is related to the subject matter described in Japanese Patent Application No. 2023-052514, filed on March 29, 2023, the entire disclosure of which is incorporated herein by reference.

[0019] INDUSTRIAL APPLICABILITY According to the present invention, it is possible to provide an actinic ray-curable ink having improved printability and curability, and to provide printed matter using the ink, which are extremely useful industrially.

[0020] Hereinafter, embodiments of the present invention will be described in detail. However, the present invention is not limited to the embodiments described below, and various modifications are possible within the scope of the gist of the present invention. In this specification, the term "(meth)acrylate" means acrylate and / or methacrylate. Furthermore, the term "(meth)acryloyl group" means acryloyl group and / or methacryloyl group. In this specification, the term "(meth)acryloyl group concentration" means the number of moles of (meth)acryloyl groups (carbon-carbon double bonds (C═C)) per gram of urethane (meth)acrylate (A). More specifically, this is the value (mmol / g) obtained by dividing the number of moles of (meth)acryloyl groups present in the urethane (meth)acrylate (A) by the mass of the urethane (meth)acrylate (A), and is a theoretical value calculated from the masses of raw materials used in producing the urethane (meth)acrylate (A).

[0021] In an embodiment of the present invention, an active energy ray-curable ink (hereinafter also referred to as "ink") contains a urethane (meth)acrylate (A) and a (meth)acrylic compound (B) other than (A), and is characterized in that the (meth)acryloyl group concentration of the urethane (meth)acrylate (A) is in the range of 4.0 to 8.0 mmol / g. When the (meth)acryloyl group concentration of the urethane (meth)acrylate (A) is in the range of 4.0 to 8.0 mmol / g, it is possible to achieve both excellent printability and curability. By ensuring that the (meth)acryloyl group concentration is 4.0 mmol / g or more, deterioration of the ink's curability can be suppressed. Furthermore, by ensuring that the (meth)acryloyl group concentration is 8.0 mmol / g or less, it is possible to suppress difficulty in introducing a structure that exhibits printability. In one embodiment, the (meth)acryloyl group concentration of the urethane (meth)acrylate (A) is preferably in the range of 4.5 to 7.5 mmol / g, more preferably in the range of 5.0 to 7.0 mmol / g.

[0022] In the active energy ray-curable ink of the above embodiment, the content of the urethane (meth)acrylate (A) is preferably 5 to 40 mass %, more preferably 10 to 30 mass %, and even more preferably 15 to 25 mass %, relative to the total amount of the ink, from the viewpoints of printability and curability.

[0023] A preferred embodiment of the urethane (meth)acrylate (A) is a reaction product of a (meth)acrylic compound (a1) having one or more hydroxyl groups, a polyol compound (a2) other than the (a1), and an isocyanate compound (a3).

[0024] ((Meth)acrylic Compound (a1) Having One or More Hydroxyl Groups) Examples of the (meth)acrylic compound (a1) having one or more hydroxyl groups include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, polyethylene glycol (meth)acrylate, caprolactone-modified 2-hydroxyethyl (meth)acrylates, glycerin poly(meth)acrylate, diglycerin poly(meth)acrylate, trimethylolpropane poly(meth)acrylate, ditrimethylolpropane poly(meth)acrylate, pentaerythritol poly(meth)acrylate, dipentaerythritol poly(meth)acrylate, and polypentaerythritol poly(meth)acrylate.

[0025] These (meth)acrylic compounds (a1) having one or more hydroxyl groups may be used alone or in combination of two or more. Among these, in order to set the (meth)acryloyl group concentration of the urethane (meth)acrylate (A) to 4.0 to 8.0 mmol / g, it is preferable to use at least one selected from the group consisting of pentaerythritol poly(meth)acrylate, dipentaerythritol poly(meth)acrylate, and polypentaerythritol poly(meth)acrylate. Furthermore, in terms of ink fluidity, it is preferable to use dipentaerythritol poly(meth)acrylate.

[0026] (Polyol Compound (a2) Other Than (a1)) As the polyol compound (a2) other than (a1), a polyol compound having two or more hydroxyl groups in the molecule can be used. It is preferable that the polyol compound (a2) does not contain a polymerizable functional group such as a (meth)acryloyl group. As the polyol compound (a2), preferably, a polyol compound having 3 to 20 carbon atoms and an alkylene oxide-modified polyol compound having 3 to 20 carbon atoms can be used. The use of these compounds improves the printability of the ink. In one embodiment, as the polyol compound (a2), more preferably, a polyol compound having a hydroxyl value in the range of 125 to 1850 mgKOH / g can be used, and the use of these compounds improves the curability of the ink. In one embodiment, the hydroxyl value of the polyol compound may be preferably 200 to 1850 mgKOH / g, more preferably 300 to 1850 mgKOH / g, and even more preferably 400 to 1850 mgKOH / g.

[0027] Specific examples of polyol compounds having 3 to 20 carbon atoms are as follows: Linear alkylene dihydric alcohols: 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,4-butanediol, 1,2-pentanediol, 1,5-pentanediol, 1,6-hexanediol, 1,2-hexanediol, 1,5-hexanediol, 2,5-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,2-octanediol, 1,9 1,10-decanediol, 1,12-dodecanediol, 1,2-dodecanediol, 1,14-tetradecanediol, 1,2-tetradecanediol, 1,16-hexadecanediol, 1,2-hexadecanediol, 1,18-octadecanediol, 1,2-octadecanediol, 1,20-eicosanediol, and 1,2-eicosanediol.

[0028] Examples of branched alkylene dihydric alcohols include neopentyl glycol, 2-methyl-2,4-pentanediol, 3-methyl-1,5-pentanediol, 2-methyl-2-propyl-1,3-propanediol, 2,4-dimethyl-2,4-dimethylpentanediol, 2,2-diethyl-1,3-propanediol, 2,2,4-trimethyl-1,3-pentanediol, dimethylol octane, 2-ethyl-1,3-hexanediol, 2,5-dimethyl-2,5-hexanediol, 2-methyl-1,8-octanediol, 2-butyl-2-ethyl-1,3-propanediol, and 2,4-diethyl-1,5-pentanediol.

[0029] Examples of cyclic alkylene dihydric alcohols include 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 1,2-cycloheptanediol, tricyclodecane dimethanol, bisphenol A, bisphenol F, bisphenol S, hydrogenated bisphenol A, hydrogenated bisphenol, and hydrogenated bisphenol S. Examples of trihydric or higher polyhydric alcohols include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, diglycerin, ditrimethylolpropane, dipentaerythritol, tripentaerythritol, sorbitan, sorbitol, and inositol.

[0030] These polyol compounds having 3 to 20 carbon atoms may be used alone or in combination of two or more. Among these, from the viewpoint of availability, it is preferable to use 1,2-propylene glycol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, glycerin, trimethylolpropane, pentaerythritol, etc.

[0031] Examples of alkylene oxide-modified polyol compounds having 3 to 20 carbon atoms include alkylene oxide-modified compounds obtained by modifying the above-mentioned polyol compounds having 3 to 20 carbon atoms with ethylene oxide (EO-modified), propylene oxide (PO-modified), butylene oxide (BO-modified), etc. The alkylene oxide-modified polyol compounds having 3 to 20 carbon atoms may be used alone or in combination of two or more.

[0032] Alkylene oxide-modified polyol compounds having 3 to 20 carbon atoms can also be obtained as commercially available products. Examples include the Sannix PP series (manufactured by Sanyo Chemical Industries, Ltd., polypropylene glycol), the PTMG series (manufactured by Mitsubishi Chemical Corporation, polytetramethylene glycol), the Uniox G series (manufactured by NOF Corporation, ethylene oxide-modified glycerin), the Sannix GP series (manufactured by Sanyo Chemical Industries, Ltd., propylene oxide-modified glycerin), the Sannix TP series (manufactured by Sanyo Chemical Industries, Ltd., propylene oxide-modified trimethylolpropane), and Wilbride S-753D (manufactured by NOF Corporation, EOPOBO-modified glycerin).

[0033] (Isocyanate Compound (a3)) The isocyanate compound (a3) ​​is not particularly limited, and any known compound having two or more isocyanate groups in the molecule can be used. For example, tolylene diisocyanate, 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, and 2,2,4-trimethylhexamethylene diisocyanate. , 2,4,4-trimethylhexamethylene diisocyanate, cyclohexane-1,4-diisocyanate, xylylene diisocyanate, isophorone diisocyanate, lysine diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, methylcyclohexane diisocyanate, m-tetramethylxylylene diisocyanate, dimer diisocyanate in which the carboxyl group of a dimer acid is converted to an isocyanate group, Millionate MR400 (manufactured by Tosoh Corporation, Polymeric MDI), and the like.

[0034] Of these compounds, from the viewpoint of reaction control, the isocyanate compound (a3) ​​is preferably a diisocyanate compound. The diisocyanate compound may be an aliphatic diisocyanate compound or an aromatic diisocyanate compound. In one embodiment, the diisocyanate compound preferably includes at least one selected from the group consisting of 4,4'-diphenylmethane diisocyanate, toluene-2,4-diisocyanate, isophorone diisocyanate, and 1,6-hexamethylene diisocyanate.

[0035] (Method for producing urethane (meth)acrylate (A)) In one embodiment, the urethane (meth)acrylate (A) preferably contains a reaction product of a (meth)acrylic compound (a1) having one or more hydroxyl groups, a polyol compound (a2) other than the (a1), and an isocyanate compound (a3). A method for producing such a reaction product will be described below.

[0036] The reaction of the (meth)acrylic compound (a1) having one or more hydroxyl groups, the polyol compound (a2) other than (a1), and the isocyanate compound (a3) ​​may be carried out simultaneously. Alternatively, the (meth)acrylic compound (a1) having one or more hydroxyl groups and the isocyanate compound (a3) ​​may be reacted in advance, and then the polyol compound (a2) may be reacted. Since the (meth)acrylic compound (a1) having one or more hydroxyl groups can be reliably reacted with the polyol compound (a2) via the isocyanate compound (a3), it is more preferable to react the (meth)acrylic compound (a1) having one or more hydroxyl groups with the isocyanate compound (a3) ​​in advance, and then react the polyol compound (a2). The ratio ((a1') / (a3')) of the number of moles of hydroxyl groups contained in the (meth)acrylic compound (a1) having one or more hydroxyl groups to the number of moles of isocyanate groups (a3') contained in the isocyanate compound (a3) ​​is preferably in the range of 0.2 to 0.6. When (a1') / (a3')) is in the range of 0.2 to 0.6, the molecular weight of the urethane (meth)acrylate (A) falls within a suitable range, which facilitates improvement of printability.

[0037] The above reaction proceeds without a catalyst, but a catalyst can also be used. Usable catalysts include, for example, tertiary amine catalysts such as triethylamine and dimethylaniline, and metal catalysts such as tin, zinc, and aluminum. In one embodiment, from the viewpoint of reactivity, it is preferable to use at least one catalyst selected from the group consisting of tin 2-ethylhexanoate, zinc acetylacetonate, and aluminum acetylacetonate. The above reaction can be carried out in a solvent as necessary, but a method of reacting in a (meth)acrylic compound (B) described below may also be applied. This method is preferred because it eliminates the steps of dissolving the urethane (meth)acrylate (A) in the (meth)acrylic compound and removing the solvent.

[0038] From the viewpoint of printability, the molecular weight of the urethane (meth)acrylate (A) is preferably in the range of 2,000 to 30,000 in terms of weight-average molecular weight. Adjusting the weight-average molecular weight to 2,000 or more tends to easily suppress problems such as ink fountain runoff due to poor ink fluidity. On the other hand, adjusting the weight-average molecular weight to 30,000 or less tends to easily suppress problems such as ink mist due to strong interactions between high-molecular-weight components in the ink. In one embodiment, the weight-average molecular weight may more preferably be 2,000 to 20,000, and even more preferably be 3,000 to 15,000. In this specification, the weight-average molecular weight is a value measured using a gel permeation chromatography (HLC-8320) manufactured by Tosoh Corporation. Specifically, a calibration curve was prepared using a standard polystyrene sample. The eluent was tetrahydrofuran, and three TSKgel Super HM-M columns (manufactured by Tosoh Corporation) were used. Measurements were performed at a flow rate of 0.6 ml / min, an injection volume of 10 μl, and a column temperature of 40° C.

[0039] The number of (meth)acryloyl groups contained in the urethane (meth)acrylate (A) is preferably 4 to 50 per molecule, more preferably 7 to 30 per molecule, from the viewpoints of printability and curability.

[0040] ((Meth)acrylic Compound (B)) The content of the (meth)acrylic compound (B) used in the ink of the above embodiment may be 10 to 90 mass % relative to the total amount of the ink, more preferably 20 to 85 mass %, and even more preferably 30 to 80 mass %.

[0041] The (meth)acrylic compound (B) is not particularly limited. Specific examples of compounds that can be used as the (meth)acrylate compound (B) include the following: monofunctional (meth)acrylic compounds such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxydipropylene glycol (meth)acrylate, phenoxyethyl (meth)acrylate, 2-(2-vinyloxyethoxy)ethyl (meth)acrylate, and acryloylmorpholine. Bifunctional (meth)acrylic compounds such as ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate (n=2 to 20), propylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate (n=2 to 20), alkane (having 4 to 12 carbon atoms) glycol di(meth)acrylate, alkane (having 4 to 12 carbon atoms) glycol ethylene oxide adduct (2 to 20 moles) di(meth)acrylate, alkane (having 4 to 12 carbon atoms) glycol propylene oxide adduct (2 to 20 moles) di(meth)acrylate, hydroxypivalyl hydroxypivalate di(meth)acrylate, tricyclodecane dimethylol di(meth)acrylate, bisphenol A ethylene oxide adduct (2 to 20 moles) di(meth)acrylate, hydrogenated bisphenol A di(meth)acrylate, and hydrogenated bisphenol A ethylene oxide adduct (2 to 20 moles) di(meth)acrylate. Trifunctional (meth)acrylic compounds such as glycerin tri(meth)acrylate, glycerin ethylene oxide adduct (3 to 30 mol) tri(meth)acrylate, glycerin propylene oxide adduct (3 to 30 mol) tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane ethylene oxide adduct (3 to 30 mol) tri(meth)acrylate, and trimethylolpropane propylene oxide adduct (3 to 30 mol) tri(meth)acrylate.tetra- or higher functional (meth)acrylic compounds such as pentaerythritol tetra(meth)acrylate, pentaerythritol ethylene oxide adduct (4 to 40 mol) tetra(meth)acrylate, pentaerythritol propylene oxide adduct (4 to 40 mol) tetra(meth)acrylate, diglycerin tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, ditrimethylolpropane ethylene oxide adduct (4 to 40 mol) tetra(meth)acrylate, ditrimethylolpropane propylene oxide adduct (4 to 40 mol) tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol ethylene oxide adduct (6 to 60 mol) hexa(meth)acrylate, and dipentaerythritol propylene oxide adduct (6 to 60 mol) hexa(meth)acrylate. Other examples include polyester (meth)acrylate, urethane (meth)acrylate other than the urethane (meth)acrylate (A) (i.e., different from (A)), and epoxy (meth)acrylate.

[0042] As the (meth)acrylic compound (B), one of the above compounds may be used alone, or two or more may be used in combination. In one embodiment, from the viewpoint of curability, it is preferable to use a bifunctional or higher (meth)acrylic compound. From the viewpoint of curability, the proportion of the bifunctional or higher (meth)acrylic compound in the total amount of the (meth)acrylic compound (B) may be in the range of preferably 40 to 100 mass%, more preferably 60 to 100 mass%, and even more preferably 90 to 100 mass%. Furthermore, in one embodiment, from the viewpoint of curability, the proportion of the tetrafunctional or higher (meth)acrylic compound in the total amount of the (meth)acrylic compound (B) may be in the range of preferably 10 to 100 mass%, more preferably 30 to 100 mass%.

[0043] In the active energy ray-curable ink of the present invention, active energy ray-curable compounds other than the above-mentioned (meth)acrylic compound (B) can be used depending on the required physical properties of the cured film.

[0044] As the active energy ray-curable compound other than (B) above (i.e., different from (B) above), for example, a vinyl compound can be used. Specific examples include styrene, N-vinylpyrrolidone, and divinylbenzene.

[0045] In one embodiment, a colored pigment can be added as a colorant to the actinic ray-curable ink, and when a colored pigment is added, the ink becomes colored. On the other hand, when no colored pigment is added, the ink becomes clear ink (also called varnish). In one embodiment, the clear ink may contain an extender pigment that does not have coloring power. In one embodiment, the colored ink may contain a colored pigment and an extender pigment.

[0046] The colored pigment may be either an inorganic pigment or an organic pigment, and various known pigments can be used. Examples of inorganic pigments include yellow lead, zinc yellow, Prussian blue, barium sulfate, cadmium red, titanium oxide, zinc white, red iron oxide, ultramarine, carbon black, graphite, aluminum powder, and red iron oxide.

[0047] Examples of organic pigments include soluble azo pigments such as β-naphthols, β-oxynaphthoic acid pigments, β-oxynaphthoic acid anilides, acetoacetate anilides, and pyrazolone pigments; insoluble azo pigments such as β-naphthols, β-oxynaphthoic acid anilides, acetoacetate anilide monoazos, acetoacetate anilide disazos, and pyrazolone pigments; phthalocyanine pigments such as copper phthalocyanine blue, halogenated (chlorinated or brominated) copper phthalocyanine blue, sulfonated copper phthalocyanine blue, and metal-free phthalocyanine; polycyclic pigments and heterocyclic pigments such as quinacridones, dioxazines, threnes (pyranthrones, anthanthrones, indanthrones, anthrapyrimidines, flavanthrones, thioindigo pigments, anthraquinones, perinones, perylenes, and the like), isoindolinones, metal complexes, and quinophthalones.

[0048] In one embodiment, the actinic radiation-curable ink may contain an extender pigment that does not have coloring power. The use of an extender pigment tends to facilitate adjustment of the ink viscosity. Examples of extender pigments include barium sulfate, magnesium silicate, alumina white, calcium carbonate, magnesium carbonate, aluminum silicate, magnesium silicate, silicon dioxide, and aluminum hydroxide.

[0049] In one embodiment, the active energy ray-curable ink may contain a resin, if necessary. Usable resins are not particularly limited. Examples include allyl resins such as diallyl orthophthalate resin, diallyl isophthalate resin, and diallyl terephthalate resin, polyester resin, polyvinyl chloride, poly(meth)acrylic acid ester, epoxy resin, polyurethane resin, petroleum (based) resin, cellulose derivatives (e.g., ethyl cellulose, cellulose acetate, nitrocellulose), vinyl chloride-vinyl acetate copolymer, polyamide resin, polyvinyl acetal resin, polyamide resin, polyvinyl acetal resin, butadiene-acrylonitrile copolymer, and the like. In one embodiment, a non-phthalate allyl resin that does not contain a phthalate structure may be used as the allyl resin. These resins may be used alone or in combination of two or more.

[0050] In one embodiment, the actinic ray-curable ink may contain a photopolymerization initiator as needed. Examples of the photopolymerization initiator include a photocleavage initiator and a hydrogen abstraction initiator.

[0051] Photocleavage initiators include acetophenone-based compounds and acylphosphine oxide-based compounds.

[0052] More specifically, examples of acetophenone compounds include 2,2-dimethoxy-2-phenylacetophenone, 2-hydroxy-2-methylpropiophenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-(dimethylamino)-1-[4-(morpholino)phenyl]-1-butanone, and 2-(dimethylamino)-2-(4-methylbenzyl)-1-[4-(morpholino)phenyl]-1-butanone, and examples of acylphosphine oxide compounds include diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and ethylphenyl(2,4,6-trimethylbenzoyl)phosphinate. These compounds may be used alone or in combination of two or more.

[0053] Furthermore, examples of the hydrogen abstraction type polymerization initiator include dialkylaminobenzophenone compounds and thioxanthone compounds.

[0054] More specifically, examples of the dialkylaminobenzophenone compound include 4,4'-dialkylaminobenzophenones such as 4,4'-bis-(dimethylamino)benzophenone and 4,4'-bis-(diethylamino)benzophenone, and 4-benzoyl-4'-methyldiphenyl sulfide. The dialkylaminobenzophenone compound may be used alone or in combination of two or more kinds.

[0055] Examples of the thioxanthone compound include 2,4-diethylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diisopropylthioxanthone, 2-isopropylthioxanthone, 4-diisopropylthioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2,4-dichlorothioxanthone, 2-chlorothioxanthone, 1-chloro-4-propoxythioxanthone, 2-hydroxy-3-(3,4-dimethyl-9-oxo-9Hthioxanthone-2-yloxy-N,N,N-trimethyl-1-propanamine hydrochloride, and the like. These may be used alone or in combination of two or more.

[0056] Sensitizers include benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 2,3,4-trimethylbenzophenone, 4-phenylbenzophenone, 3,3'-dimethyl-4-methoxybenzophenone, 4-(1,3-acryloyl-1,4,7,10,13-pentaoxotridecyl)benzophenone, methyl-o-benzoylbenzoate, [4-(methylphenylthio)phenyl]phenylmethanone, (4-benzoylbenzyl)trimethylammonium chloride, 2-hydroxy- Examples include 2-methyl-1-phenylpropan-1-one, 1-(4-isopropylphenyl)2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexylphenyl ketone, 2-hydroxy-2-methyl-1-styrylpropan-1-one polymers, diethoxyacetophenone, dibutoxyacetophenone, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin normal butyl ether, etc. These may be used alone or in combination of two or more.

[0057] The active energy ray-curable ink of the present invention may contain other additives as required.

[0058] A radical polymerization inhibitor can be added as an additive to impart storage stability to the ink. Examples of radical polymerization inhibitors include (alkyl)phenols, hydroquinone, catechol, resorcinol, p-methoxyphenol, t-butylcatechol, t-butylhydroquinone, pyrogallol, 1,1-picrylhydrazyl, phenothiazine, p-benzoquinone, nitrosobenzene, 2,5-di-tert-butyl-p-benzoquinone, dithiobenzoyl disulfide, picric acid, cupferron, aluminum N-nitrosophenylhydroxylamine, tri-p-nitrophenylmethyl, N-(3-oxyanilino-1,3-dimethylbutylidene)aniline oxide, dibutyl cresol, cyclohexanone oxime cresol, guaiacol, o-isopropylphenol, butyraldoxime, methyl ethyl ketoxime, and cyclohexanone oxime.

[0059] Waxes can also be added as additives to impart abrasion resistance, anti-blocking properties, smoothness, and scratch resistance, including natural waxes such as carnauba wax, Japan wax, lanolin, montan wax, paraffin wax, and microcrystalline wax, and synthetic waxes such as Fischer-Tropsch wax, polyethylene wax, polypropylene wax, polytetrafluoroethylene wax, polyamide wax, and silicone compounds.

[0060] In addition, additives such as ultraviolet absorbers, infrared absorbers, antibacterial agents, etc. may be added to the active energy ray-curable ink depending on the required performance.

[0061] The active energy ray-curable ink of the above embodiment may have a composition consisting of 0 to 30 mass % of pigment, 5 to 40 mass % of urethane (meth)acrylate (A), 20 to 80 mass % of (meth)acrylic compound (B), 0 to 30 mass % of resin, 0 to 20 mass % of photopolymerization initiator and / or sensitizer, and 0 to 10 mass % of other additives, relative to the total mass of the ink, and can be adjusted by blending predetermined amounts of raw materials.

[0062] In printing inks, organic solvents are generally used as viscosity modifiers. However, the use of organic solvents is becoming increasingly restricted due to concerns about environmental impact and operational safety. In contrast, the active energy ray-curable ink of the above-described embodiment preferably contains substantially no organic solvent. By containing substantially no organic solvent, it is possible to provide an active energy ray-curable ink that is free of volatile components (non-VOCs), which has a low environmental impact and excellent operational safety. Here, "substantially no organic solvent" means that the ink is not intentionally added as a constituent component and that the content due to unintentional addition is less than 1% by mass. Examples of unintentional addition include trace amounts contained in each raw material and trace amounts contained as contamination during the ink manufacturing process and the printed matter production process.

[0063] The actinic energy ray-curable ink of the above embodiment can be produced by applying the same method as that for conventional actinic energy ray-curable inks. For example, the ink can be produced by kneading and mixing ink composition components including raw materials such as the pigment, urethane (meth)acrylate (A), (meth)acrylic compound (B), polymerization inhibitor, photopolymerization initiator and sensitizer, and other additives at a temperature between room temperature and 100° C. using a preparation machine such as a kneader, a three-roll mill, an attritor, a sand mill, or a gate mixer.

[0064] In one embodiment, the method for producing the active energy ray-curable ink may include a step of preparing a urethane (meth)acrylate (A). For example, the production method may include a step of reacting a (meth)acrylic compound (a1) having one or more hydroxyl groups with a polyol compound (a2) other than (a1), and an isocyanate compound (a3) ​​to obtain the urethane (meth)acrylate (A). In one embodiment, the reaction is preferably carried out in the presence of a (meth)acrylic compound (B) that constitutes the ink. The (meth)acrylic compound (B) is as described above.

[0065] One embodiment of the present invention relates to a printed matter having a substrate and a printed layer provided on at least one main surface of the substrate, the printed layer being formed from a cured product of the active energy ray-curable ink of the embodiment. The printed matter can be produced, for example, by a known method including printing (applying) the active energy ray-curable ink of the embodiment to at least one surface of the substrate to form a coating film, and irradiating the coating film with active energy rays to cure the coating film.

[0066] In the method for producing the printed matter, the method for printing or applying the active energy ray-curable ink onto a substrate is not particularly limited. For example, applicable methods include a roll coater, gravure coater, flexo coater, air doctor coater, blade coater, air knife coater, squeeze coater, impregnation coater, transfer roll coater, kiss coater, curtain coater, cast coater, spray coater, die coater, offset printing, flexo printing, gravure printing, and screen printing. In one embodiment, offset printing is preferred. The offset printing may be either conventional offset printing, which uses dampening water, or waterless offset printing, which does not use dampening water.

[0067] The substrate of the printed matter is not particularly limited, and examples include printing on any material such as paper, plastic, stickers, labels, metal, etc. In one embodiment, the printed matter may be obtained by printing ink onto a paper substrate.

[0068] In the method for producing the printed matter, the method for curing the ink with actinic radiation is not particularly limited, and any known actinic radiation source can be used, including, for example, a mercury lamp, a xenon lamp, a metal hydride lamp, LEDs (light-emitting diodes) such as ultraviolet light-emitting diodes (UV-LEDs) and ultraviolet laser diodes (UV-LDs), electron beams, gas, and solid-state lasers.

[0069] The present invention will be described in more detail below with reference to examples, but the following examples do not limit the scope of the invention in any way. In the present invention, "parts" means "parts by mass" and "%" means "% by mass".

[0070] (Production Example 1) In a four-neck flask equipped with a stirrer, a cooler, a thermometer, and a gas inlet tube, 70.9 parts of MIRAMER M500 (a mixture with the (meth)acrylic compound (B) component described below) as a (meth)acrylic compound (a1) having one or more hydroxyl groups, 11.8 parts of toluene-2,4-diisocyanate as an isocyanate compound (a3), 9.6 parts of MIRAMER M600 and 5.0 parts of LAROMER LR8863 as a (meth)acrylic compound (B), 0.01 parts of tin 2-ethylhexanoate as a catalyst, and 0.2 parts of tertiary butylhydroquinone as a polymerization inhibitor were added, and the mixture was stirred and air was blown in to react for 1 hour at 100 ° C. Next, 2.6 parts of propylene glycol was added as a polyol compound (a2) other than (a1), and the mixture was further reacted at 110 ° C. for 5 hours to obtain a resin composition 1 containing urethane acrylate. In this reaction, the value of [(a1') / (a3')] was 0.5, and the concentration of (meth)acrylic groups in the resulting urethane acrylate was 6.79 mmol / g.

[0071] (Production Examples 2 to 30, 33 to 38, 40) Resin compositions 2 to 30, 33 to 38, and 40 were obtained in the same manner as in Production Example 1, except that the raw materials were changed according to the formulations in Table 1.

[0072] (Production Example 31) Into a four-neck flask equipped with a stirrer, a cooler, a thermometer, and a gas inlet tube, 71.6 parts of MIRAMER M500 (a mixture with a (meth)acrylic compound (B) described later) as a (meth)acrylic compound (a1) having one or more hydroxyl groups, 2.1 parts of glycerin as a polyol compound (a2) other than (a1), 11.9 parts of toluene-2,4-diisocyanate as an isocyanate compound (a3), 9.2 parts of MIRAMER M600 and 5.0 parts of LAROMER LR8863 as a (meth)acrylic compound (B), 0.01 parts of tin 2-ethylhexanoate as a catalyst, and 0.2 parts of tert-butylhydroquinone as a polymerization inhibitor were placed, and air was blown in with stirring, followed by a reaction at 110°C for 5 hours to obtain a resin composition 31 containing urethane acrylate. In this reaction, the value of [(a1') / (a3')] was 0.5, and the concentration of (meth)acrylic groups in the resulting urethane acrylate was 6.86 mmol / g.

[0073] (Production Example 32) Resin composition 32 was obtained in the same manner as in Production Example 31, except that the raw materials were changed according to the composition in Table 1.

[0074] (Production Example 39) Into a four-neck flask equipped with a stirrer, a condenser, a thermometer, and a gas inlet tube, 92.1 parts of MIRAMER M500 (a mixture with the (meth)acrylic compound (B) described below) as the (meth)acrylic compound (a1) having one or more hydroxyl groups, 7.7 parts of toluene-2,4-diisocyanate as the isocyanate compound (a3), 0.01 parts of tin 2-ethylhexanoate as a catalyst, and 0.2 parts of tert-butylhydroquinone as a polymerization inhibitor were placed, and air was blown in with stirring, allowing the mixture to react at 100°C for 5 hours to obtain a urethane acrylate-containing resin composition 39. The value of [(a1') / (a3')] in this reaction was 1.0, and the (meth)acrylic group concentration of the resulting urethane acrylate was 8.18 mmol / g.

[0075]

[0076]

[0077] Details of the materials listed in Table 1 are described below. (Meth)acrylic compounds (a1) ARONIX M306: manufactured by Toagosei Co., Ltd., a mixture of pentaerythritol triacrylate / pentaerythritol tetraacrylate = 70 / 30 (mass ratio) MIRAMER M500: manufactured by Bigen Specialty Chemical Co., Ltd., a mixture of dipentaerythritol pentaacrylate / dipentaerythritol hexaacrylate = 50 / 50 (mass ratio) Viscoat #802: manufactured by Osaka Organic Chemical Industry Ltd., polypentaerythritol polyacrylate HEA: manufactured by Osaka Organic Chemical Industry Ltd., 2-hydroxyethyl acrylate 4-HBA: manufactured by Osaka Organic Chemical Industry Ltd., 4-hydroxybutyl acrylate

[0078] Polyol compounds (a2) Sannix PP-600: manufactured by Sanyo Chemical Industries, Ltd., polypropylene glycol; PTMG-250: manufactured by Mitsubishi Chemical Corporation, polytetramethylene glycol; Uniox G-450: manufactured by NOF Corporation, ethylene oxide-modified glycerin; Sannix GP-250: manufactured by Sanyo Chemical Industries, Ltd., propylene oxide-modified glycerin; Sannix TP-400: manufactured by Sanyo Chemical Industries, Ltd., propylene oxide-modified trimethylolpropane; Wilbride S-753D: manufactured by NOF Corporation, EOPOBO-modified glycerin; Newpol BP-2P: manufactured by Sanyo Chemical Industries, Ltd., propylene oxide-modified bisphenol A; Newpol BPE-20T: manufactured by Sanyo Chemical Industries, Ltd., ethylene oxide-modified bisphenol A; Sannix PP-1200: manufactured by Sanyo Chemical Industries, Ltd., polypropylene glycol Isocyanate compound (a3) ​​Millionate MR400: Polymeric MDI (diphenylmethane diisocyanate), manufactured by Tosoh Corporation

[0079] (Meth)acrylic compound (B) MIRAMER M600: dipentaerythritol hexaacrylate manufactured by Bigen Specialty Chemical Co., Ltd. LAROMER LR8863: ethylene oxide-modified trimethylolpropane triacrylate manufactured by BASF

[0080] Polymerization inhibitor TBHQ: tertiary butyl hydroquinone

[0081] (Examples 1 to 34, Comparative Examples 1 to 8) The actinic ray-curable inks of Examples 1 to 34 and Comparative Examples 1 to 8 were obtained by using the previously prepared urethane acrylate-containing resin compositions 1 to 40, blending the raw materials according to the formulations in Table 2, and milling the mixture in a three-roll mill. To evaluate the printability of the obtained actinic ray-curable inks, "ink mist" and "ink fountain run-off" were measured on a printing press. To evaluate curability, "wet heat blocking" of the printed matter was measured. These results are all shown in Table 2.

[0082] <Method of measuring ink mist> Printing was carried out at a speed of 10,000 sheets per hour using an offset sheet-fed printing press LITHRONE L426 (Komori Corporation) under the following conditions. During printing, a blank sheet of paper was attached to the inside of the safety cover of the printing press, and after 10,000 passes, the blank sheet was removed and the degree of ink scattering was evaluated. "A", "B", and "C" represent practical levels. (Evaluation criteria) A: A small amount of ink mist is scattered on a part of the white paper B: A thin layer of ink mist is scattered over the entire surface of the white paper C: A somewhat thick layer of ink mist is scattered over the entire surface of the white paper D: A thick layer of ink mist is scattered over the entire surface of the white paper (Printing conditions) Printing press: LITHRONE 26 (Komori Corporation) Paper: OK Topcoat+ (79.1 g / m), manufactured by Oji Paper Co., Ltd. 2 ) Printing speed: 10,000 sheets / hour Lamp: Eye Graphics metal halide lamp (output 120W / cm, 1 lamp used)

[0083] <Method of evaluating ink fountain run-off> The ink fountain was observed during printing in the same manner as above to see if there was any trouble with "ink fountain run-off," in which the ink was not scraped off by the supply roller. "A," "B," and "C" are practical levels. (Evaluation criteria) A: No trouble occurs for 60 minutes or more B: No trouble occurs for 30 minutes or more but less than 60 minutes C: No trouble occurs for 10 minutes or more but less than 30 minutes D: Trouble occurs in less than 10 minutes

[0084] <Method for evaluating wet heat blocking> The ink was applied to coated paper (OK Top Coat Plus manufactured by Oji Paper Co., Ltd.) at a rate of 1 g / m using an RI tester (simple color development machine). 2 The ink was applied (printed) with a coating amount of 1000 ppm. The ink-printed surface of the coated paper was irradiated with a metal halide lamp (manufactured by iGraphics Co., Ltd.) to harden the ink and obtain a printed matter. The irradiation conditions were output: 96 W / cm, lamp distance: 10 cm, and the irradiation time was adjusted by changing the conveyor speed (80, 100, 120 m / min). Next, the printed matter was cut into a 4 cm x 5 cm square to prepare a test piece. The ink-printed surfaces of the test pieces were placed together and then heated at a temperature of 40°C, humidity of 80% RH, and a load of 2 kg / cm. 2 After blocking for 24 hours, the condition of the printed matter was evaluated. The evaluation criteria are as follows: "A", "B" and "C" are practical levels. (Evaluation criteria) A: No change in the printed surface B: Peeling is observed on part of the printed surface (less than 10% of the area) C: Peeling is observed on part of the printed surface (10% or more but less than 50% of the area) D: Peeling is observed on part of the printed surface (50% or more of the area) or the entire printed surface

[0085]

[0086]

[0087]

[0088]

[0089] Details of the materials listed in Table 2 are given below. Pigment Carbon black: Carbon black MA11 manufactured by Mitsubishi Chemical Corporation Photopolymerization initiator Omnirad379EG: 2-(dimethylamino)-2-(4-methylbenzyl)-1-[4-(morpholino)phenyl]-1-butanone manufactured by iGM RESINS KAYACURE DETX-S: 2,4-diethylthioxanthone manufactured by Nippon Kayaku Co., Ltd.

[0090] The content (mass%) of urethane acrylate in the ink shown in Table 2 is a value calculated based on the content of urethane acrylate in the resin composition calculated from the total amount of the reactive component having a hydroxyl group in (a1), component (a2), and component (a3) ​​used as raw materials during production.

[0091] Examples 1 to 32, which are embodiments of the present invention, contain inks containing urethane acrylates with (meth)acryloyl group concentrations within the range of 4.0 to 8.0 mmol / g, and were evaluated as being good in terms of "ink mist," "ink fountain runoff," and "humid heat blocking." On the other hand, Comparative Examples 1 to 8 contain inks containing urethane acrylates with (meth)acryloyl group concentrations outside the above range. Comparative Examples 7 and 8 showed poor ink mist evaluations due to reduced ink elasticity. Furthermore, Comparative Examples 1 to 6 and 8 showed poor ink fluidity due to the urethane acrylates having (meth)acryloyl group concentrations of less than 4.0 mmol / g, resulting in poor evaluations of moist heat blocking. Furthermore, Comparative Examples 1 to 4 and 7 showed poor ink flowability and ink fountain runoff. These findings demonstrate that the present invention provides an active energy ray-curable ink that can suppress ink mist and ink fountain runoff, has excellent curability, and can eliminate printing problems.

Claims

1. An active energy ray-curable ink containing a urethane (meth)acrylate (A) and a (meth)acrylic compound (B) other than (A), wherein the (meth)acryloyl group concentration of the urethane (meth)acrylate (A) is in the range of 4.0 to 8.0 mmol / g.

2. The active energy ray-curable ink according to claim 1, wherein the urethane (meth)acrylate (A) is a reaction product of a (meth)acrylic compound (a1) having one or more hydroxyl groups, a polyol compound (a2) other than the (a1), and an isocyanate compound (a3).

3. The active energy ray-curable ink according to claim 2, wherein the (meth)acrylic compound (a1) having one or more hydroxyl groups includes at least one selected from the group consisting of pentaerythritol poly(meth)acrylate, dipentaerythritol poly(meth)acrylate, and polypentaerythritol poly(meth)acrylate.

4. The active energy ray-curable ink according to claim 2, wherein the polyol compound (a2) comprises at least one selected from the group consisting of polyol compounds having 3 to 20 carbon atoms and alkylene oxide-modified polyol compounds having 3 to 20 carbon atoms.

5. The active energy ray-curable ink according to claim 2, wherein the polyol compound (a2) is at least one selected from the group consisting of propylene glycol, butanediol, neopentyl glycol, hexanediol, octanediol, decanediol, glycerin, trimethylolpropane, pentaerythritol, and alkylene oxide modified products thereof.

6. The active energy ray-curable ink according to claim 2, wherein the polyol compound (a2) has a hydroxyl value of 125 to 1850 mg KOH / g.

7. The active energy ray-curable ink according to claim 2, wherein the isocyanate compound (a3) ​​is a diisocyanate compound.

8. The active energy ray-curable ink according to claim 2, wherein the ratio [(a1') / (a3')] of the number of moles (a1') of hydroxyl groups contained in the (meth)acrylic compound (a1) having one or more hydroxyl groups to the number of moles (a3') of isocyanate groups contained in the isocyanate compound (a3) ​​is in the range of 0.2 to 0.

6.

9. A method for producing an active energy ray-curable ink according to claim 1, comprising the step of reacting a (meth)acrylic compound (a1) having one or more hydroxyl groups, a polyol compound (a2) other than said (a1), and an isocyanate compound (a3) ​​in a (meth)acrylic compound (B) to obtain a urethane (meth)acrylate (A).

10. A printed matter having a substrate and a cured product of the active energy ray-curable ink according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Thiadiazole IRAK4 inhibitors

    JP2023052514A

  • High surface-area lyophilized compositions comprising arsenic for oral administration in patients

    JP2024161468A

  • Active energy ray-curable composition, active energy ray-curable printing ink using same, and print

    WO2016063625A1

  • Ultraviolet curable ink composition for ink-jet recording

    JP2004027211A

  • Active energy beam-curable coating composition

    JP2006249353A