Recyclable sheet

The recyclable sheet, featuring a cyclodextrin-based undercoat layer with improved solvent solubility, addresses the challenge of recyclability by detaching functional layers from base materials, enabling efficient reuse of the base materials through solvent immersion.

WO2024202546A1PCT designated stage expired Publication Date: 2024-10-03LINTEC CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/003798
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-02-06
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current materials and technologies do not effectively address the recyclability of products with functional layers, specifically failing to facilitate the removal of these layers from base materials for reuse.

Method used

A recyclable sheet is developed with an undercoat layer containing a cyclodextrin compound, which is soluble in solvents, allowing the functional layer to be detached from the base material, enabling the base material to be reused. The undercoat layer has a low film density and excellent solvent solubility, with the cyclodextrin compound being preferably substituted with acyl groups and combined with an acrylic monomer for improved properties.

Benefits of technology

The recyclable sheet effectively detaches the functional layer from the base material when immersed in a solvent, allowing for the reuse of the base material, thus enhancing recyclability and reducing waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024003798_03102024_PF_FP_ABST
    Figure JP2024003798_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A recyclable sheet 1 comprises: a base material 11; an undercoat layer 12 provided on at least one surface side of the base material 11; and a functional layer 13 provided on the undercoat layer 12 on the opposite side from the base material 11. The undercoat layer 12 contains a cyclodextrin compound. The gel fraction of the materials constituting the undercoat layer 12 is preferably at most 20%. The undercoat layer 12 preferably contains the cyclodextrin compound as a monomer, and preferably further contains an acrylic monomer. By using the recyclable sheet 1, it is possible to recycle the base material.
Need to check novelty before this filing date? Find Prior Art

Description

Recyclable sheet

[0001] The present invention relates to a recyclable sheet whose substrate can be recycled.

[0002] In recent years, there has been an increasing demand for the creation of a recycling-based society, and there is a growing demand for recyclability of various products and materials.

[0003] For example, when a product in which a predetermined coating (e.g., a functional layer having a predetermined function) is formed on a substrate made of plastic or the like is discarded, it may be possible to reuse the substrate by removing the coating from the substrate.

[0004] Patent Document 1 aims to provide a film-forming material (film-forming composition) that can easily detach a film from a substrate such as a general-purpose plastic substrate by a simple method using neutral water, and that can easily remove a film layer from the substrate. The film-forming composition contains a release promoter, and the release promoter has a functional group that is hydrophilic, and the functional group is protected by a protecting group, and the hydrophilic property is exhibited when the protecting group is deprotected by a treatment such as heating.

[0005] Recently, novel materials using cyclodextrin monomers have been proposed. Specifically, Patent Document 2 proposes a polymer material containing a crosslinked polymer crosslinked by the interaction between a host group and a guest group, in which the host group is a monovalent group obtained by removing one hydrogen atom or one hydroxyl group from cyclodextrin, and the crosslinked polymer contains a predetermined repeating structural unit.

[0006] Furthermore, Patent Document 3 proposes an inclusion complex formed from a host group of a host group-containing monomer and a guest group of a guest group-containing monomer, in which the host group-containing monomer is a cyclodextrin monomer derivative having a (meth)acryloyl group, and the guest group-containing monomer is a predetermined monomer having a vinyl group.

[0007] JP 2022-183764 A Japanese Patent No. 6636610 A Japanese Patent No. 6239043 A

[0008] However, Patent Documents 2 and 3 make no mention of removal of the coating (functional layer) from the substrate or recyclability.

[0009] The present invention has been made in view of the above circumstances, and has an object to provide a recyclable sheet whose substrate can be recycled.

[0010] In order to achieve the above object, first, the present invention provides a recyclable sheet comprising a substrate, an undercoat layer provided on at least one side of the substrate, and a functional layer provided on the undercoat layer on the side opposite the substrate, wherein the undercoat layer contains a cyclodextrin compound (Invention 1).

[0011] In the above invention (Invention 1), the undercoat layer containing a cyclodextrin compound, which is a cyclic molecule having an opening, has a low coating density and excellent solvent solubility. Therefore, by immersing the recyclable sheet in a predetermined solvent, the undercoat layer dissolves in the solvent, and the undercoat layer and the functional layer are detached from the substrate. This allows the substrate to be reused.

[0012] In the above invention (Invention 1), it is preferable that the gel fraction of the material constituting the undercoat layer is 20% or less (Invention 2).

[0013] In the above inventions (Inventions 1 and 2), it is preferable that the undercoat layer contains the cyclodextrin compound as a monomer (Invention 3).

[0014] In the above inventions (Inventions 1 to 3), the cyclodextrin compound is preferably a compound in which some or all of the hydroxyl groups of cyclodextrin have been substituted with acyl groups (Invention 4).

[0015] In the above inventions (Inventions 1 to 4), it is preferable that the undercoat layer contains an acrylic monomer (Invention 5).

[0016] In the above inventions (Inventions 1 to 5), the content of the cyclodextrin compound in the undercoat layer is preferably 0.01% by mass or more and 30% by mass or less (Invention 6).

[0017] In the above inventions (Inventions 1 to 6), it is preferable that the thickness of the undercoat layer is 0.01 μm or more and 10 μm or less (Invention 7).

[0018] In the above inventions (Inventions 1 to 7), it is preferable that the functional layer is a release agent layer and the recyclable sheet is a release sheet (Invention 8).

[0019] The recyclable sheet according to the present invention allows the substrate to be recycled.

[0020] 1 is a cross-sectional view of a recyclable sheet according to one embodiment of the present invention.

[0021]

[0013] Hereinafter, an embodiment of the present invention will be described. A recyclable sheet according to one embodiment of the present invention comprises a substrate, an undercoat layer provided on at least one side of the substrate, and a functional layer provided on the undercoat layer on the side opposite to the substrate, wherein the undercoat layer contains a cyclodextrin compound. A specific configuration of one example of the recyclable sheet according to this embodiment is shown in Figure 1.

[0022] As shown in FIG. 1, the recyclable sheet 1 according to this embodiment comprises, from the bottom up, a substrate 11, an undercoat layer 12 laminated on the substrate 11, and a functional layer 13 laminated on the undercoat layer 12.

[0023] 1. Elements (1) Substrate The substrate 11 in the recyclable sheet 1 according to the present embodiment is not particularly limited as long as it is resistant to the solvent for dissolving the undercoat layer 12, and can be appropriately selected depending on the application of the recyclable sheet 1.

[0024] Specifically, examples of the substrate 11 include polyester films such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyolefin films such as polyethylene and polypropylene; cellophane; diacetyl cellulose film; triacetyl cellulose film; acetyl cellulose butyrate film; polyvinyl chloride film; polyvinylidene chloride film; polyvinyl alcohol film; ethylene-vinyl acetate copolymer film; ethylene-(meth)acrylic acid copolymer film; ethylene-(meth)acrylic acid ester copolymer film; polystyrene film; polycarbonate film; polymethylpentene film; and polysulfone film. Examples of suitable plastic films include plastic films such as polyether ether ketone films, polyethersulfone films, polyetherimide films, fluororesin films, polyamide films, polyimide films, acrylic resin films, polyurethane resin films, ionomer resin films, norbornene polymer films, cyclic olefin polymer films, cyclic conjugated diene polymer films, and vinyl alicyclic hydrocarbon polymer films, or laminated films thereof; woven or nonwoven fabrics made of fibers such as rayon, acrylic, and polyester; papers such as fine paper, glassine paper, impregnated paper, and coated paper; metal foils such as aluminum and copper; foams such as urethane foam and polyethylene foam; and laminates of two or more of these.

[0025] From the perspective of the SDGs, the material constituting the substrate 11 may be a material with a high biomass content, a material that can be recycled or reused, or a recycled or reused material.

[0026] The thickness of the substrate 11 varies depending on its type and application, but is usually preferably 10 to 200 μm, more preferably 20 to 160 μm, particularly preferably 30 to 120 μm, even more preferably 40 to 100 μm, and of these, preferably 45 to 80 μm.

[0027] (2) Undercoat Layer The undercoat layer 12 in the recyclable sheet 1 according to this embodiment preferably contains a cyclodextrin compound. Cyclodextrin compounds are cyclic molecules with openings. By containing a cyclodextrin compound having such a structure, the undercoat layer 12 has a reduced coating density, improved swelling and wetting properties with solvents, and excellent solvent solubility. Therefore, by immersing the recyclable sheet 1 according to this embodiment in a predetermined solvent, the undercoat layer 12 dissolves in the solvent, and the undercoat layer 12 and the functional layer 13 are detached from the substrate 11. This allows the substrate 11 to be reused. In this way, the recyclable sheet 1 according to this embodiment has excellent substrate recyclability. The solvent used during recycling will be described later.

[0028] The cyclodextrin compound may be cyclodextrin itself, cyclodextrin having a substituent (cyclodextrin derivative), or cyclodextrin or a cyclodextrin derivative incorporated into a polymer (a polymer having cyclodextrin or a cyclodextrin derivative as a constituent monomer), but it is preferably present in the undercoat layer 12 in the form of a monomer. This improves the solvent solubility of the undercoat layer 12. In other words, the cyclodextrin compound is preferably cyclodextrin itself or a cyclodextrin having a substituent (cyclodextrin derivative).

[0029] The cyclodextrin skeleton of the cyclodextrin compound is preferably α-cyclodextrin, β-cyclodextrin, or γ-cyclodextrin, and among these, β-cyclodextrin or γ-cyclodextrin is preferred from the viewpoint of better solvent solubility. Furthermore, from the viewpoint of solvent solubility, the cyclodextrin compound preferably has a substituent. Therefore, the cyclodextrin compound is particularly preferably β-cyclodextrin or γ-cyclodextrin having a substituent.

[0030] The above-mentioned substituent is a group obtained by substituting a hydroxyl group of cyclodextrin. Examples of the above-mentioned substituent include an acyl group, an alkyl group, a trityl group, a tosyl group, a trimethylsilane group, a phenyl group, an amide group, a (meth)acryloyl group, etc.; (meth)acrylamide, N-monoalkyl(meth)acrylamide, N-dialkyl(meth)acrylamide, etc.; a polyester chain, an oxyethylene chain, an alkyl chain, an ether chain, an ester chain, an acrylic ester chain, etc. In this specification, (meth)acryl means both acryl and methacryl. The same applies to other similar terms.

[0031] The cyclodextrin compound is preferably a compound in which some or all of the hydroxyl groups of cyclodextrin are substituted with acyl groups, and the acyl groups are particularly preferably acetyl groups, which improves the solvent solubility of the undercoat layer 12.

[0032] In the cyclodextrin compound, it is preferable that no hydroxyl groups remain in the cyclodextrin, and it is more preferable that some of the hydroxyl groups are substituted with (meth)acrylamide or a derivative thereof, and all of the remaining hydroxyl groups are substituted with acyl groups, particularly acetyl groups. It is even more preferable that one hydroxyl group is substituted with (meth)acrylamide or a derivative thereof, and all of the remaining hydroxyl groups are substituted with acyl groups, particularly acetyl groups. Preferred examples of (meth)acrylamide derivatives include N-monoalkyl(meth)acrylamides and N-dialkyl(meth)acrylamides, with N-methyl(meth)acrylamide being particularly preferred, and N-methylacrylamide being even more preferred. This improves the solvent solubility of the undercoat layer 12.

[0033] The content of the cyclodextrin compound in the undercoat layer 12 is preferably 0.01 to 30% by mass, more preferably 0.3 to 20% by mass, particularly preferably 0.6 to 10% by mass, and even more preferably 0.9 to 5% by mass. This improves the solvent solubility of the undercoat layer 12. Furthermore, other components, such as the acrylic monomers described below, can be contained in appropriate amounts, which can improve the functionality of the components, such as film strength.

[0034] In this embodiment, the undercoat layer 12 preferably does not contain guest molecules that can be included in the cyclodextrin compound. In this specification, "inclusion" refers to the phenomenon in which a guest molecule is captured within a cavity of a host molecule (cyclodextrin compound). In addition, "guest molecule" refers to a molecule that can be included in a cyclodextrin compound, including those that have not yet been included. Examples of such guest molecules include n-butyl acrylate, styrene, octyl acrylate, and dodecyl acrylate for α-cyclodextrin compounds; n-butyl acrylate, t-butyl acrylate, styrene, adamantyl acrylate, and isobornyl acrylate for β-cyclodextrin compounds; and octyl acrylate and dodecyl acrylate for γ-cyclodextrin compounds.

[0035] In this specification, the undercoat layer "does not contain guest molecules that can be included in a cyclodextrin compound" means that the undercoat layer does not substantially contain any guest molecules. Specifically, the undercoat layer is allowed to contain guest molecules in an amount of 0.1% by mass or less, preferably 0.01% by mass or less, particularly preferably 0.001% by mass or less, and even more preferably 0.0001% by mass or less.

[0036] The undercoat layer 12 preferably contains an acrylic monomer in addition to the cyclodextrin compound. This improves the film strength of the undercoat layer 12, and allows the functional layer 13 to be favorably formed and supported on the undercoat layer 12. The acrylic monomer may be used alone or in combination of two or more.

[0037] The acrylic monomer is preferably a monofunctional acrylic monomer, and particularly preferably a (meth)acrylic acid ester. This improves the film strength of the undercoat layer 12 while improving the solvent solubility of the undercoat layer 12. From the perspective of the SDGs, the acrylic monomer may be one with a high biomass content, one that is recyclable or reusable, or one that has been recycled or reused.

[0038] Examples of (meth)acrylic acid esters include (meth)acrylic acid alkyl esters in which the alkyl group is linear or branched, (meth)acrylic acid esters having a cyclic structure such as an alicyclic structure, and (meth)acrylic acid esters having a functional group such as a hydroxyl group. Among these, (meth)acrylic acid alkyl esters in which the alkyl group is linear or branched are preferred, and (meth)acrylic acid alkyl esters in which the alkyl group is linear are particularly preferred.

[0039] From the viewpoints of film strength and solvent solubility, the (meth)acrylic acid alkyl ester is preferably a (meth)acrylic acid alkyl ester having an alkyl group containing 1 to 20 carbon atoms. Examples of (meth)acrylic acid alkyl esters having an alkyl group containing 1 to 20 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, and stearyl (meth)acrylate. Among these, from the viewpoint of improving solvent solubility, the number of carbon atoms in the alkyl group is preferably 1 to 8, more preferably 1 to 6, particularly preferably 1 to 4, and even more preferably 1 to 2. Specifically, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, etc. are preferred, with methyl (meth)acrylate or ethyl (meth)acrylate being particularly preferred, and methyl acrylate or ethyl acrylate being even more preferred.

[0040] The content of the acrylic monomer in the undercoat layer 12 is preferably 70 to 99.9 mass %, more preferably 80 to 99.6 mass %, particularly preferably 90 to 99.3 mass %, and even more preferably 95 to 99.1 mass %, which provides good film strength and also improves solvent solubility.

[0041] The undercoat layer 12 preferably contains substantially only the cyclodextrin compound and the acrylic monomer, although it may contain components other than the cyclodextrin compound and the acrylic monomer as long as they do not impair the function of the undercoat layer 12. Specifically, the total content of the cyclodextrin compound and the acrylic monomer in the undercoat layer 12 is preferably 50% by mass or more, more preferably 75% by mass or more, particularly preferably 90% by mass or more, even more preferably 95% by mass or more, and of these, preferably 99% by mass or more, and most preferably 100% by mass.

[0042] The molar ratio of the acrylic monomer to the cyclodextrin compound in the undercoat layer 12 is preferably 50:50 to 99.9:0.1, more preferably 75:25 to 99.5:0.5, particularly preferably 80:20 to 99.2:0.8, and even more preferably 85:15 to 99.1:0.9, which allows for a good balance between excellent solvent solubility and good film strength.

[0043] The gel fraction of the material (composition) constituting the undercoat layer 12 is preferably 20% or less, more preferably 15% or less, particularly preferably 10% or less, even more preferably 7% or less, and most preferably 5% or less. The lower limit of the gel fraction is preferably 0%. This improves the solvent solubility of the undercoat layer 12. The method for measuring the gel fraction in this specification is as shown in the test examples described below.

[0044] The thickness of the undercoat layer 12 is preferably 0.01 to 10 μm, more preferably 0.03 to 6 μm, particularly preferably 0.06 to 3 μm, further preferably 0.09 to 1 μm, and most preferably 0.1 to 0.7 μm, which allows for a good balance between excellent solvent solubility and good film strength.

[0045] (3) Functional Layer The functional layer 13 in the recyclable sheet 1 according to this embodiment is a layer having a desired function. Examples of the functions of the functional layer 13 include, but are not limited to, peelability, hard coating properties (scratch resistance), self-repairing properties, reflectivity, semi-transparency, anti-reflection properties, anti-glare properties, fingerprint resistance, easy slippage, anti-static properties, improvement of writing feel, anti-Newton ring properties, colorability, light diffusion properties, specific wavelength blocking properties, design properties, and anti-fogging properties.

[0046] Among the above-mentioned functions, the functional layer 13 preferably has releasability, that is, the functional layer 13 is preferably a release layer. In this case, the recyclable sheet 1 can be used as a release sheet. Release sheets are usually discarded after being peeled from the layer that they protect, such as a pressure-sensitive adhesive layer, an adhesive layer, a hard coat layer, a self-repairing layer, a writing feel improving layer, a ceramic green sheet, etc. However, if the recyclable sheet 1 according to this embodiment is used as a release sheet, the substrate 11 can be recycled even after peeling (use).

[0047] The release layer can be formed using a release agent. The type of release agent is not particularly limited, and examples thereof include silicone-based, fluorine-based, alkyd-based, melamine resin-based, unsaturated polyester-based, polyolefin-based, and wax-based release agents.

[0048] As the silicone-based release agent, for example, one containing an addition reaction type silicone resin obtained from a first organopolysiloxane having at least two alkenyl groups (e.g., vinyl groups) in one molecule and a second organopolysiloxane (corresponding to a crosslinking agent) having at least two hydrosilyl groups in one molecule, and a silicone resin can be preferably used. As the silicone resin, for example, a monofunctional siloxane unit [(CH 3 ) 3 SiO 1/2 ] and a tetrafunctional siloxane unit [SiO 4/2In the silicone-based release agent described above, the hardness of the release agent layer can be adjusted by the skeleton of the addition reaction type silicone resin, and the surface polarity can be adjusted by the amount of silicone resin added, thereby making it possible to obtain the desired surface free energy and releasability.

[0049] The thickness of the functional layer 13 varies depending on its type and application, but is usually preferably 0.01 to 100 μm, more preferably 0.04 to 60 μm, particularly preferably 0.08 to 20 μm, and even more preferably 0.1 to 10 μm. In particular, when the functional layer 13 is a release layer, its thickness is preferably 0.2 to 7 μm, more preferably 0.4 to 4 μm, particularly preferably 0.6 to 3 μm, and even more preferably 0.8 to 2 μm.

[0050] 2. Manufacturing Method To manufacture the recyclable sheet 1 according to this embodiment, first, an undercoat layer 12 is formed on the substrate 11. To form the undercoat layer 12, it is preferable to first prepare a coating liquid of a material (composition) that constitutes the undercoat layer 12.

[0051] Specifically, a coating liquid is obtained by mixing a cyclodextrin compound, and optionally an acrylic monomer, a diluting solvent, and the like.

[0052] Examples of the dilution solvent include aliphatic hydrocarbons such as hexane, heptane, and cyclohexane; aromatic hydrocarbons such as toluene and xylene; halogenated hydrocarbons such as methylene chloride and ethylene chloride; alcohols such as methanol, ethanol, propanol, butanol, and 1-methoxy-2-propanol; ketones such as acetone, methyl ethyl ketone, 2-pentanone, isophorone, and cyclohexanone; esters such as ethyl acetate and butyl acetate; and cellosolve-based solvents such as ethyl cellosolve.

[0053] The concentration and viscosity of the coating solution are not particularly limited as long as they are within a range that allows coating, and can be appropriately selected depending on the situation. For example, the coating solution is diluted so that the concentration of the composition in the coating solution is 10 to 40 mass %. Note that the addition of a dilution solvent or the like is not a necessary condition for obtaining the coating solution, and as long as the composition has a viscosity that allows coating, the addition of a dilution solvent is not necessary.

[0054] Once the coating liquid for the undercoat layer 12 is obtained, the coating liquid is applied onto the substrate 11 and the coating layer is dried to form the undercoat layer 12. Examples of coating methods that can be used include gravure coating, bar coating, spray coating, spin coating, knife coating, roll coating, and die coating.

[0055] When drying the coating layer, a heat treatment may be carried out. When the heat treatment is carried out, the heating temperature is preferably 50 to 150° C., and more preferably 70 to 110° C. The heating time is preferably 10 seconds to 10 minutes, and more preferably 30 seconds to 2 minutes.

[0056] After the undercoat layer 12 is formed as described above, the functional layer 13 is then formed on the undercoat layer 12. The functional layer 13 can be formed by a known method depending on the type, material, etc. of the functional layer 13. Here, an example in which the functional layer 13 is a release layer will be described.

[0057] To form the release layer, a coating solution of the release agent that constitutes the release layer is prepared. Specifically, the release agent (each component) and, if desired, additives, a dilution solvent, etc. are mixed to obtain a release agent coating solution. The obtained release agent coating solution is applied to the undercoat layer 12, and the coating layer is cured to form the release layer. The dilution solvent and coating method are the same as those for the undercoat layer 12.

[0058] The method for curing the coated layer of release agent may be appropriately selected depending on the type of release agent, and may include thermal curing by heat treatment or active energy ray curing by irradiation with active energy rays.

[0059] In the case of thermal curing, the heating temperature is preferably 50 to 160° C., and particularly preferably 70 to 130° C. The heating time is preferably 10 seconds to 10 minutes, and particularly preferably 30 seconds to 3 minutes.

[0060] In the case of active energy ray curing, ultraviolet rays, electron beams, etc. are usually used as the active energy rays, and ultraviolet rays are particularly preferred. The irradiation dose of the active energy rays varies depending on the type of energy rays, but for example, in the case of ultraviolet rays, the light dose is 50 to 1000 mJ / cm. 2 is preferred, and particularly 100 to 500 mJ / cm 2 In the case of electron beams, the dose is preferably about 0.1 to 50 kGy.

[0061] 3. Recycling Method When recycling the recyclable sheet 1 according to this embodiment, it is preferable to immerse the recyclable sheet 1 in a solvent that easily dissolves the undercoat layer 12 but does not easily dissolve the substrate 11. As a result, the undercoat layer 12 dissolves in the solvent, and the undercoat layer 12 and the functional layer 13 are detached from the substrate 11. As a result, the substrate 11 can be reused.

[0062] Examples of solvents that can be used to dissolve the undercoat layer 12 during recycling include aliphatic hydrocarbons such as hexane, heptane, and cyclohexane; aromatic hydrocarbons such as toluene and xylene; halogenated hydrocarbons such as methylene chloride and ethylene chloride; alcohols such as methanol, ethanol, propanol, butanol, and 1-methoxy-2-propanol; ketones such as acetone, methyl ethyl ketone, 2-pentanone, isophorone, and cyclohexanone; esters such as ethyl acetate and butyl acetate; and cellosolve-based solvents such as ethyl cellosolve.

[0063] The time for immersing the recyclable sheet 1 in the solvent varies depending on the size of the recyclable sheet 1 and the type and thickness of the functional layer 13, but is preferably 0.5 to 48 hours, more preferably 1 to 36 hours, particularly preferably 1.5 to 24 hours, and even more preferably 2 to 12 hours. This allows the time until the undercoat layer 12 and the functional layer 13 are detached from the substrate 11 to be relatively short, which contributes to shortening the recycling process time.

[0064] The above-described embodiments have been described to facilitate understanding of the present invention, and are not intended to limit the present invention. Therefore, each element disclosed in the above embodiments is intended to include all design modifications and equivalents that fall within the technical scope of the present invention.

[0065] For example, another layer may be provided on the undercoat layer 12 side of the functional layer 13 or on the opposite side of the undercoat layer 12 of the functional layer 13. Furthermore, the substrate 11 may be made up of multiple layers, and another layer that remains on the substrate 11 side even after immersion in the solvent may be provided between the substrate 11 and the undercoat layer 12.

[0066] In this specification, when it is stated that "X to Y" (X and Y are any numbers), it means "X or more and Y or less" unless otherwise specified, and also means "preferably greater than X" or "preferably smaller than Y". Furthermore, when it is stated that "X or more" (X is any number), it means "preferably greater than X" unless otherwise specified, and when it is stated that "Y or less" (Y is any number), it also means "preferably smaller than Y" unless otherwise specified.

[0067] The present invention will be explained in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0068] [Production Example 1] 15 g of β-cyclodextrin and 2.0 g of N-hydroxymethylacrylamide were dissolved in 100 mL of dimethylformamide. 500 mg of para-toluenesulfonic acid monohydrate was added to the solution, and the mixture was stirred at 80°C for 30 minutes. The solution was then allowed to cool and added dropwise to 500 mL of acetone, and the resulting precipitate was collected by filtration. The resulting solid was purified by HPLC, yielding 2.9 g of a white solid.

[0069] 2.9 g of the white solid was dissolved in 80 mL of pyridine together with 25 g of acetic anhydride. The solution was then stirred at 55°C for 12 hours and then added dropwise to 300 mL of purified water. The resulting precipitate was dried under reduced pressure to obtain 3.5 g of a white solid. A portion of the white solid was dissolved in deuterated chloroform. 1 The solid was analyzed by H-NMR (product name "Nuclear Magnetic Resonance Spectrometer JNM-LA400 / WB" manufactured by JEOL Ltd.). As a result of the analysis, it was found that the white solid was a cyclodextrin compound in which one hydroxyl group in β-cyclodextrin had been substituted with N-methylacrylamide and the remaining hydroxyl groups had all been substituted with acetyl groups. This cyclodextrin compound was designated as cyclodextrin compound (CD2).

[0070] [Production Example 2] 1.8 g of β-cyclodextrin (manufactured by Nacalai Tesque) and 47 mg of p-toluenesulfonic acid monohydrate as a catalyst were added to 8.5 ml of isopropenyl acetate as a solvent, and the mixture was reacted for 16 hours at 70° C. The reaction solution was evaporated under reduced pressure, and the resulting solid was washed with a 10% by mass aqueous solution of sodium carbonate, extracted with chloroform, and recrystallized with acetone to obtain 2.5 g of acetylated β-cyclodextrin as a white solid.

[0071] A portion of the obtained acetylated β-cyclodextrin was dissolved in deuterated chloroform, 1 Analysis was performed using H-NMR (manufactured by JEOL Ltd., product name "Nuclear Magnetic Resonance Spectrometer JNM-LA400 / WB"). 1The degree of modification was calculated to be 2.98 from the integral ratio of the peak due to the proton attached to the first carbon of the glucose ring at around 5.1 ppm in the H-NMR chart to the peak due to the acetyl group at around 2.1 ppm. This acetylated β-cyclodextrin was designated as cyclodextrin compound (CD3).

[0072] Example 1 1. Preparation of coating solution for undercoat composition A cyclodextrin compound (manufactured by Yushiro Chemical Industry Co., Ltd., product name "Wizard Monomer ACCD-S") was prepared in which one hydroxyl group in β-cyclodextrin was substituted with acrylamide and all of the remaining hydroxyl groups were substituted with acetyl groups. This cyclodextrin compound is referred to as cyclodextrin compound (CD1).

[0073] 100 mol % of methyl acrylate as an acrylic monomer and 1 mol % of the above cyclodextrin compound (CD1) were mixed in ethyl acetate and thoroughly stirred to obtain a coating liquid of a composition for an undercoat layer (undercoat composition).

[0074] 2. Preparation of Release Agent Coating Liquid 100 parts by mass of an addition-type release agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KS-847H"), 15 parts by mass of an addition-type silicone resin (manufactured by Dow-Toray Industries, Inc., product name "DOWSIL SD-4584"), 2.0 parts by mass of a curing catalyst (manufactured by Dow-Toray Industries, Inc., product name "DOWSIL SRX 212 Catalyst"), and toluene as a diluent were mixed and thoroughly stirred to obtain a release agent coating liquid for forming a release layer as a functional layer.

[0075] 3. Production of recyclable sheet The coating solution of the undercoat composition obtained in step 1 above was applied using a coater to the surface opposite the easy-adhesion layer of a polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name "Cosmoshine A4160", thickness: 50 μm) having an easy-adhesion layer on one side as a substrate. The film was then dried by heating at 70 ° C. for 60 seconds to form an undercoat layer with a thickness of 0.1 μm. The thickness of the undercoat layer was measured in accordance with JIS K7130 using a constant pressure thickness gauge (manufactured by Teclock Co., Ltd., product name "PG-02") (the same applies below).

[0076] Next, the release agent coating solution obtained in step 2 was applied to the exposed surface of the undercoat layer using a coater. The coating was then heat-treated at 120°C for 120 seconds to thermally cure the coating layer, forming a release layer (R1) with a thickness of 1 μm. In this way, a recyclable sheet consisting of a release layer (1 μm) / undercoat layer (0.1 μm) / substrate (50 μm) was produced.

[0077] Examples 2, 4 to 7, Comparative Examples 1 to 3 Recyclable sheets were produced in the same manner as in Example 1, except that the type of acrylic monomer, the type of cyclodextrin compound, and the thickness of the undercoat layer were changed as shown in Table 1. In Comparative Example 3, dimethylol-tricyclodecane diacrylate was used instead of the cyclodextrin compound, and the blending amount was set to 0.2 mol%.

[0078] Example 3 100 parts by weight of dipentaerythritol hexaacrylate, 5 parts by weight of polydimethylsiloxane (manufactured by Dow-Toray Industries, Inc., product name "SH28"), and 5 parts by weight of a photopolymerization initiator (manufactured by BASF, product name "Irgacure 904") were mixed and thoroughly stirred to obtain a release agent coating solution for forming a release layer as a functional layer.

[0079] The release agent coating solution was applied to the exposed surface of the undercoat layer formed on the substrate in the same manner as in Example 1. The coating layer was then irradiated with active energy rays (ultraviolet rays; UV) under the following conditions to cure the coating layer and form a release layer (R2) with a thickness of 1 μm. In this way, a recyclable sheet consisting of release layer (1 μm) / undercoat layer (0.1 μm) / substrate (50 μm) was produced.

[0080] <Activated energy ray irradiation conditions> - High pressure mercury lamp used - Illuminance 200 mW / cm 2 , light intensity 500mJ / cm 2 ・UV illuminance and light intensity meter used is "UVPF-A1" manufactured by iGraphics

[0081] [Comparative Example 4] A laminate sheet (sometimes referred to as a "recyclable sheet" for convenience) was produced in the same manner as in Example 1, except that an undercoat layer was not formed. The laminate sheet consisted of a release layer (1 μm) and a substrate (50 μm).

[0082] [Comparative Example 5] A laminate sheet (sometimes referred to as a "recyclable sheet" for convenience) was produced in the same manner as in Example 2, except that a release layer was not formed. The laminate sheet consisted of an undercoat layer (0.5 μm) / a substrate (50 μm).

[0083] Details of the abbreviations and the like in Table 1 are as follows: [Acrylic monomers] MA: methyl acrylate EA: ethyl acrylate DCP: dimethylol-tricyclodecane diacrylate [Cyclodextrin compounds] CD1: cyclodextrin compound (manufactured by Yushiro Chemical Industry Co., Ltd., product name "Wizard Monomer ACCD-S") CD2: cyclodextrin compound produced in Production Example 1 CD3: cyclodextrin compound produced in Production Example 2

[0084] [Test Example 1] (Measurement of gel fraction) The coating solution of the undercoat composition prepared in the Examples and Comparative Examples (except Comparative Example 4) was applied by a coater to the release-treated surface of a release sheet prepared by treating one side of a polyethylene terephthalate film with a silicone-based release agent. The film was then dried by heating at 70°C for 60 seconds to form an undercoat layer with a thickness of 50 µm.

[0085] The laminated sheet consisting of the undercoat layer / release sheet prepared as described above was cut into a size of 80 mm x 80 mm. The undercoat layer (undercoat composition) was then wrapped in a polyester mesh (mesh size 200), and its mass was weighed using a precision balance. The mass of the mesh alone was subtracted to calculate the mass of the undercoat composition alone. This mass was designated M1.

[0086] Next, the undercoat composition wrapped in the polyester mesh was immersed in ethyl acetate at room temperature (23°C) for 24 hours. The undercoat composition was then removed and air-dried for 24 hours in an environment of 23°C and 50% relative humidity, and then further dried in an oven at 80°C for 12 hours. After drying, its mass was weighed using a precision balance, and the mass of the undercoat composition alone was calculated by subtracting the mass of the mesh alone. This mass was designated M2. The gel fraction (%) was expressed as (M2 / M1) x 100. The gel fraction of the undercoat composition was calculated from this. The results are shown in Table 2.

[0087] Test Example 2 (Evaluation of Scratch Resistance and Adhesion to Substrate) The surface of the release layer (undercoat layer in Comparative Example 5) of the recyclable sheets produced in the Examples and Comparative Examples was subjected to a load of 380 g / cm using a nonwoven fabric (manufactured by Asahi Kasei Corporation, product name "Bencotto"). 2 The sample was rubbed back and forth 10 times at a speed of 100 mm / s. The state of the release layer and undercoat layer was then visually inspected, and the scratch resistance and adhesion to the substrate were evaluated according to the following criteria. The results are shown in Table 2. ⊚: No scratches or peeling on the release layer or undercoat layer. ◯: Scratches on the release layer or undercoat layer, but no peeling. △: Scratches on the release layer or undercoat layer, with partial peeling. ×: Peeling of the release layer or undercoat layer occurred.

[0088] Test Example 3 (Measurement of Peel Force) A 25 mm wide adhesive tape (manufactured by Nitto Denko Corporation, product name "No. 31B") was applied to the surface of the release layer (undercoat layer in Comparative Example 5) of the recyclable sheets produced in the Examples and Comparative Examples using a 5 kg roller, and then stored for 24 hours to serve as a sample for measuring peel force. The sample was fixed to a universal tensile tester (manufactured by Shimadzu Corporation, product name "Autograph AGS-20NX"), and the adhesive tape was peeled from the release agent layer in a 180° direction at a tensile speed of 0.3 m / min in accordance with JIS K6854:1999 to measure the peel force (initial; mN / 25 mm) of the recyclable sheet. The results are shown in Table 2.

[0089] Test Example 4 (Evaluation of Solvent Immersion Removal Properties) The recyclable sheets produced in the Examples and Comparative Examples were cut into samples measuring 10 cm x 7 cm. The samples were immersed in methyl ethyl ketone at room temperature (23°C) for 2 hours, then removed and air-dried.

[0090] The surface of the release layer (undercoat layer in Comparative Example 5) in the recyclable sheet obtained as described above after solvent immersion was measured for peel strength (mN / 25 mm after solvent immersion) in the same manner as in Test Example 3. The results are shown in Table 2.

[0091] The rate of change in release force after solvent immersion relative to the initial release force measured above (rate of change in release force = (release force after solvent immersion / initial release force) x 100 (%)) was calculated. The solvent immersion releasability of the release layer and undercoat layer of the recyclable sheet was then evaluated based on the following criteria. A large rate of change in release force means that the degree of release of the release layer (and undercoat layer) was large. The results are shown in Table 2. ◯: The rate of change in release force was 2000% or more. △: The rate of change in release force was 200% or more but less than 2000%. ×: The rate of change in release force was less than 200%.

[0092]

[0093]

[0094] As can be seen from Table 2, the recyclable sheets of the Examples had excellent solvent immersion releasability of the release layer (and undercoat layer), and therefore had excellent recyclability of the substrate.

[0095] The recyclable sheet according to the present invention can be suitably used as a release sheet, for example.

[0096] DESCRIPTION OF SYMBOLS 1...Recyclable sheet 11...Substrate 12...Undercoat layer 13...Functional layer

Claims

1. A recyclable sheet comprising a substrate, an undercoat layer provided on at least one side of the substrate, and a functional layer provided on the undercoat layer on the side opposite the substrate, wherein the undercoat layer contains a cyclodextrin compound.

2. The recyclable sheet according to claim 1, characterized in that the material constituting the undercoat layer has a gel fraction of 20% or less.

3. The recyclable sheet according to claim 1, wherein the undercoat layer contains the cyclodextrin compound as a monomer.

4. The recyclable sheet according to claim 1, wherein the cyclodextrin compound is a compound in which some or all of the hydroxyl groups of cyclodextrin have been substituted with acyl groups.

5. The recyclable sheet according to claim 1, wherein the undercoat layer contains an acrylic monomer.

6. The recyclable sheet according to claim 1, characterized in that the content of the cyclodextrin compound in the undercoat layer is 0.01% by mass or more and 30% by mass or less.

7. The recyclable sheet according to claim 1, wherein the thickness of the undercoat layer is 0.01 μm or more and 10 μm or less.

8. The recyclable sheet according to any one of claims 1 to 7, characterized in that the functional layer is a release agent layer, and the recyclable sheet is a release sheet.

Citation Information

Patent Citations

  • α-Cyanoacrylate adhesive composition

    JP1993505835A

  • Pressure sensitive adhesive containing cyclodextrin

    JP2003507536A

  • Adhesive and multilayer film having the adhesive

    JP2016098323A

  • Polyester film for producing optical film

    JP2017043694A

  • Window film and manufacturing method therefor

    JP2019137716A