Multilayer resin sheet

The multilayer resin sheet addresses surface smoothness and adhesion issues in printed wiring boards by optimizing etching rates and filler distributions, ensuring effective desmear treatment and maintaining film thickness, thus improving wiring formation and simplifying the manufacturing process.

WO2024202564A1PCT designated stage expired Publication Date: 2024-10-03AJINOMOTO CO INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/004160
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-02-07
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The existing build-up manufacturing method for printed wiring boards faces issues with surface smoothness and adhesion during conductor layer formation due to resin residue in via holes, requiring additional processes like desmear treatment and mold release agent cleaning.

Method used

A multilayer resin sheet with specific etching rates and filler particle size distributions ensures smooth surface finish and reduced smear even after desmear treatment, maintaining film thickness and adhesion without the need for additional cleaning steps.

Benefits of technology

The multilayer resin sheet provides an insulating layer with good surface smoothness, well-shaped via holes, and minimal film thickness change, enhancing the formation of fine wiring and reducing process complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

Provided is a novel technique capable of providing an insulating layer that has good surface smoothness and comprises a via hole having a reduced smear and a good shape, even when desmear treatment is performed after a support is peeled off. This multilayer resin sheet comprises two or more layers of resin composition layers having a first resin composition layer which is one outermost layer and a layer excluding the first resin composition layer, wherein: RD / RA is 5 or more and less than 100, where the etching rate of a cured product of the first resin composition layer by a desmear treatment is RA, and the etching rate of a cured product of a resin composition layer which is the outermost layer on the opposite side from the first resin composition layer by a desmear treatment is RD; and the arithmetic average roughness Ra of the cured product of the first resin composition layer after desmear treatment is less than 50 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Multilayer resin sheet

[0001] The present invention relates to a multilayer resin sheet. It also relates to a multilayer resin sheet with a support, a printed wiring board, and a semiconductor device obtained using the multilayer resin sheet. The present invention also relates to a method for producing a printed wiring board using the multilayer resin sheet.

[0002] A known manufacturing technique for printed wiring boards is a build-up manufacturing method in which insulating layers and conductor layers (circuit layers) are alternately stacked. In build-up manufacturing methods, insulating layers are generally formed by laminating a resin composition layer on a circuit board using a resin sheet or the like containing a resin composition layer and curing the resin composition layer. For example, Patent Document 1 discloses a technique in which a resin composition layer is laminated on a circuit board using a resin sheet having a plurality of resin composition layers, the resin composition layer is thermally cured to obtain a cured product, and then the cured product is roughened to form a thin insulating layer with excellent mechanical strength.

[0003] WO 2009 / 119621

[0004] In the technology described in Patent Document 1, when via holes are formed with a laser to form wiring, a desmearing process must be performed to remove resin residue (smear) in the via holes, but increasing the intensity of the desmearing process to improve the ability to remove smears in the via holes can roughen the resin surface and impair the smoothness of the insulating layer surface. If the insulating layer surface has poor smoothness, when a conductor layer (wiring layer) is formed on the insulating layer, adhesion between the pattern-forming dry film and the insulating layer is likely to decrease, which can result in poor formation of fine wiring.

[0005] To solve this problem, a technique has been proposed in which via holes are formed with a laser while the insulating layer surface is protected by a support, and then the support is peeled off after a desmear treatment. This technique makes it possible to remove smears in the via holes while maintaining a smooth insulating layer surface. However, this technique requires peeling off the support after the desmear treatment, which is problematic in that it requires a change from the conventional process. Another problem is that the release agent remains on the insulating layer surface after the support is peeled off, which requires a separate step to wash off the release agent.

[0006] The present invention provides a novel technique that can provide an insulating layer having good surface smoothness, reduced smearing, and well-shaped via holes, even when a desmear treatment is performed after peeling off the support.

[0007] As a result of extensive research into the above problems, the present inventors have found that the above problems can be solved by a multilayer resin sheet having the following configuration, and have thus completed the present invention.

[0008] That is, the present invention includes the following: <1> A multilayer resin sheet having two or more resin composition layers consisting of a first resin composition layer that is one outermost layer and a layer other than the first resin composition layer, wherein, where RA is the etching rate in a desmear treatment of a cured product of the first resin composition layer and RD is the etching rate in a desmear treatment of a cured product of the resin composition layer that is the outermost layer on the side opposite the first resin composition layer, RD / RA is 5 or more and less than 100, and the arithmetic mean roughness Ra of the cured product of the first resin composition layer after the desmear treatment is less than 50 nm. <2> The multilayer resin sheet according to <1>, wherein, when D1 is the average particle size (μm) of the inorganic filler in the first resin composition layer and D2 is the average particle size (μm) of the inorganic filler in the layer other than the first resin composition layer, D1 < D2. <3> The multilayer resin sheet according to <1> or <2>, wherein the content of the inorganic filler in the first resin composition layer is 5% by mass or less, when the total amount of non-volatile components in the first resin composition layer is 100% by mass. <4> The multilayer resin sheet according to any one of <1> to <3>, wherein the etching rate RA is 0.1% or more and less than 1%. <5> The multilayer resin sheet according to any one of <1> to <4>, wherein, when the thickness (μm) of the multilayer resin sheet is T and the thickness (μm) of the first resin composition layer is t, t<(T-t). <6> The multilayer resin sheet according to any one of <1> to <5>, which is used by being laminated on a target member such that the surface opposite to the first resin composition layer is joined to the target member. <7> The multilayer resin sheet according to any one of <1> to <6>, which is used for an insulating layer of a printed wiring board. <8> A multilayer resin sheet with a support, comprising the multilayer resin sheet according to any one of <1> to <7> and a support bonded to the first resin composition layer of the multilayer resin sheet. <9> A method for producing a printed wiring board, comprising the following steps (I) to (IV):(I) a step of laminating the multilayer resin sheet according to any one of <1> to <7> on an inner layer substrate so that the surface of the multilayer resin sheet opposite to the first resin composition layer is joined to the inner layer substrate, (II) a step of curing the multilayer resin sheet to form an insulating layer, (III) a step of forming via holes in the insulating layer with a laser and performing a desmear treatment, and (IV) a step of forming a metal film on the surface of the insulating layer after the desmear treatment. <10> A printed wiring board comprising an insulating layer made of a cured product of the multilayer resin sheet according to any one of <1> to <7>. <11> A semiconductor device comprising the printed wiring board according to <10>.

[0009] According to the present invention, it is possible to provide a novel technique that can provide an insulating layer having a good surface smoothness, reduced smearing, and well-shaped via holes, even when a desmear treatment is performed after peeling off the support.

[0010] According to the present invention, even when the desmear treatment is carried out after the support is peeled off, an insulating layer can be obtained with little change in film thickness before and after the desmear treatment.

[0011] The present invention will be described in detail below with reference to preferred embodiments thereof. However, the present invention is not limited to the following embodiments and examples, and can be implemented with any modifications within the scope of the claims of the present invention and their equivalents.

[0012] [Multilayer Resin Sheet] The multilayer resin sheet of the present invention comprises two or more resin composition layers including a first resin composition layer as one outermost layer and a layer other than the first resin composition layer, and is characterized in that, when RA is the etching rate by a desmear treatment of a cured product of the first resin composition layer and RD is the etching rate by a desmear treatment of a cured product of the resin composition layer that is the outermost layer on the opposite side to the first resin composition layer, RD / RA is 5 or more and less than 100, and Ra of the cured product of the first resin composition layer after the desmear treatment is less than 50 nm.

[0013] The multilayer resin sheet of the present invention has a structure in which two or more resin composition layers are laminated on top of each other. Here, in a multilayer resin sheet having a structure in which two resin composition layers, a first resin composition layer and a second resin composition layer, are laminated, both the first resin composition layer and the second resin composition layer are outermost layers. Furthermore, in a multilayer resin sheet having a structure in which N resin composition layers (where N is an integer of 3 or more) are laminated, when numbers are assigned in ascending order from one outermost layer to the other outermost layer as 1st, 2nd, ..., Nth, the first resin composition layer and the Nth resin composition layer are the outermost layers.

[0014] The multilayer resin sheet of the present invention is used by laminating it to a member to be laminated (e.g., an inner layer substrate, as described below). In this case, the surface opposite to the first resin composition layer, which is one of the outermost layers (the other outermost layer; in a multilayer resin sheet consisting of two resin composition layers, this corresponds to the second resin composition layer, and in a multilayer resin sheet consisting of N resin composition layers, this corresponds to the Nth resin composition layer) is bonded to the member to be laminated. Therefore, when laminated to the member to be laminated, the first resin composition layer faces the outside (external environment), and therefore, hereinafter, the first resin composition layer may be simply referred to as the "outer layer." Furthermore, of the multiple resin composition layers constituting the multilayer resin sheet of the present invention, the layers other than the first resin composition layer are positioned between the first resin composition layer and the member to be laminated after lamination to the member to be laminated. Therefore, hereinafter, the layers other than the first resin composition layer may be collectively referred to as the "inner layer."

[0015] In the multilayer resin sheet of the present invention, the resin composition layers may be two or more layers, or may be three or more layers. Note that the multilayer resin sheet of the present invention may be formed by causing differences in the contents of each component in a substantially single resin sheet. In this case, the portion where the contents of each component differ can be considered to be the layer interface.

[0016] The multilayer resin sheet of the present invention is characterized in that, when RA is the etching rate in a desmear treatment of a cured product of the first resin composition layer, which is one of the outermost layers, and RD is the etching rate in a desmear treatment of a cured product of the resin composition layer, which is the outermost layer on the opposite side to the first resin composition layer, RD / RA is 5 or more and less than 100. As a result, even when a desmear treatment is performed after peeling off the support, the multilayer resin sheet of the present invention can provide an insulating layer with good surface smoothness, reduced smearing, and well-shaped via holes. Furthermore, even when a desmear treatment is performed after peeling off the support, the multilayer resin sheet of the present invention can provide an insulating layer with little change in film thickness before and after the desmear treatment.

[0017] In the present invention, the "etching rate by desmear treatment of a cured product" of a resin composition layer refers to a mass reduction rate (% by mass) calculated by the formula: [(M'-M") / M'] x 100, where M' is the mass of the cured product of the resin composition layer before desmear treatment and M" is the mass of the cured product of the resin composition layer after desmear treatment. Therefore, the etching rate RA by desmear treatment of a cured product of a first resin composition layer can be calculated by the formula: [(MA'-MA") / MA'] x 100, where MA' is the mass of the cured product of the first resin composition layer before desmear treatment and MA" is the mass of the cured product of the first resin composition layer after desmear treatment. Furthermore, the etching rate RD by desmear treatment of the cured product of the resin composition layer which is the outermost layer opposite to the first resin composition layer can be calculated by the formula: [(MD'-MD") / MD']×100, where MD' is the mass of the cured product of the resin composition layer which is the outermost layer opposite to the first resin composition layer before desmear treatment and MD" is the mass of the cured product of the resin composition layer which is the outermost layer opposite to the first resin composition layer after desmear treatment. Here, the "resin composition layer which is the outermost layer opposite to the first resin composition layer" corresponds to the second resin composition layer in a multilayer resin sheet consisting of two resin composition layers, and corresponds to the Nth resin composition layer in a multilayer resin sheet consisting of N resin composition layers.

[0018] In the present invention, the etching rates RA and RD can be measured according to the method described later in the section [Measurement of Etching Rate]. Specifically, in a case where a target resin composition layer is thermally cured by heating at 100°C for 30 minutes and then at 170°C for 30 minutes, and the resulting cured product is subjected to a desmear treatment by immersing it in a swelling liquid at 60°C for 10 minutes, in an oxidizing agent liquid at 80°C for 20 minutes, and in a neutralizing liquid at 40°C for 10 minutes, the etching rates RA and RD can be determined by measuring the mass of the cured product before and after the desmear treatment and substituting the results into the above formula.

[0019] Even when a desmear treatment is carried out after peeling off the support, from the viewpoint of providing an insulating layer having good surface smoothness, reduced smears, and well-shaped via holes, it is important that the etching rate RA is sufficiently smaller than the etching rate RD, and the RD / RA ratio is 5 or more, preferably 5.5 or more or 6 or more, more preferably 6.5 or more or 7 or more, and even more preferably 8 or more, 9 or more, 10 or more, 12 or more, 14 or more, or 15 or more. An RD / RA ratio of 10 or more is particularly preferred because it is likely to provide an insulating layer having particularly good surface smoothness.

[0020] Even when a desmear treatment is performed after peeling off the support, from the viewpoint of obtaining an insulating layer having good surface smoothness, reduced smears, and well-shaped via holes, it is important that the etching rate RD is not too large compared with the etching rate RA, and the RD / RA ratio is less than 100, preferably 98 or less, 96 or less, or 95 or less, more preferably 94 or less, 92 or less, 90 or less, 88 or less, or 86 or less, and even more preferably 85 or less, 84 or less, 82 or less, or 80 or less. In particular, an RD / RA ratio of 85 or less is preferable because it is easy to obtain an insulating layer having particularly well-shaped via holes with little dimensional change in the thickness direction of the insulating layer while suitably reducing smears.

[0021] Even when the desmear treatment is performed after peeling off the support, from the viewpoint of providing an insulating layer having better surface smoothness, reduced smears, and well-shaped via holes, and further from the viewpoint of being able to provide an insulating layer with little change in film thickness before and after the desmear treatment, it is preferable that the RD / RA ratio be within a specific range, and that the etching rate RA of the cured product of the first resin composition layer by the desmear treatment be preferably 1% or less or less than 1%, more preferably 0.9% or less, more preferably 0.85% or less or 0.8% or less, even more preferably 0.75% or less, 0.7% or less, 0.65% or less, 0.6% or less, or 0.55% or less, still more preferably 0.5% or less, 0.48% or less, 0.46% or less, 0.45% or less, 0.44% or less, 0.42% or less, or 0.4% or less, and the lower limit thereof is preferably 0.05% or more, more preferably 0.06% or more or 0.08% or more, and even more preferably 0.1% or more. Therefore, in a preferred embodiment, the etching rate RA is equal to or greater than 0.1% and less than 1%.

[0022] The etching rate RD of the cured product of the resin composition layer that is the outermost layer opposite the first resin composition layer by the desmear treatment is not limited as long as the RD / RA ratio is within the above-mentioned specific range in relation to the etching rate RA. In particular, since it is easy to obtain an insulating layer having via holes with a particularly good shape (cross-sectional shape) with little dimensional change in the thickness direction of the insulating layer while suitably reducing smear, the etching rate RD is preferably 20% or less, more preferably 18% or less, 16% or less, or 15% or less, even more preferably 14% or less, 12% or less, or 10% or less, and even more preferably less than 10%, 9.5% or less, or 9% or less, and the lower limit thereof is preferably 0.5% or more, more preferably 0.6% or more or 0.8% or more, and even more preferably 1% or more, 1.2% or more, 1.4% or more, or 1.5% or more.

[0023] In the multilayer resin sheet of the present invention, the first resin composition layer, which is one of the outermost layers, provides a cured product with low surface roughness and excellent surface smoothness when subjected to a desmear treatment after curing. In the multilayer resin sheet of the present invention, the cured product of the first resin composition layer has an arithmetic mean roughness Ra of less than 50 nm after desmear treatment. If the cured product of the first resin composition layer has an Ra of less than 50 nm after desmear treatment, even if the thickness of the metal film provided thereon as a plating seed layer is made thinner, plating burn during wiring formation is suppressed and a uniform conductor layer (wiring) is easily formed, which is advantageous from the perspective of fine wiring. The Ra of the cured product of the first resin composition layer after desmear treatment may be even smaller, preferably 45 nm or less, 40 nm or less, or 35 nm or less, and more preferably 30 nm or less, 28 nm or less, 26 nm or less, or 25 nm or less. The lower limit of Ra is not particularly limited and may be, for example, 1 nm or more, 2 nm or more, or 3 nm or more.

[0024] In the present invention, the Ra of the cured product of the first resin composition layer after the desmear treatment can be measured according to the method described later in the section "Measurement of Surface Roughness." Specifically, the first resin composition layer is thermally cured by heating at 100°C for 30 minutes and then at 170°C for 30 minutes, and the resulting cured product is subjected to a desmear treatment by immersing it in a swelling liquid at 60°C for 10 minutes, in an oxidizing agent liquid at 80°C for 20 minutes, and in a neutralizing liquid at 40°C for 10 minutes. The arithmetic mean roughness Ra of the cured product of the first resin composition layer after the desmear treatment is measured.

[0025] In the multilayer resin sheet of the present invention, the layers other than the first resin composition layer preferably contain an inorganic filler from the viewpoint of obtaining a cured product having a low linear thermal expansion coefficient and a low dielectric loss tangent (and thus a cured product having low transmission loss when operated in a high-frequency environment). Details of the inorganic filler will be described later.

[0026] In the multilayer resin sheet of the present invention, the first resin composition layer may or may not contain an inorganic filler. In one embodiment, the first resin composition layer contains an inorganic filler from the viewpoint of providing a cured product with a low linear thermal expansion coefficient and a low dielectric loss tangent. When the first resin composition layer contains an inorganic filler, the inorganic filler contained in the first resin composition layer preferably has a smaller average particle size than the inorganic filler contained in layers other than the first resin composition layer from the viewpoint of providing a cured product with even lower surface roughness and better smoothness after desmearing. Therefore, in a preferred embodiment, when the average particle size (μm) of the inorganic filler in the first resin composition layer is D1 and the average particle size (μm) of the inorganic filler in layers other than the first resin composition layer is D2, D1 < D2. From the viewpoint of further enjoying the effects of the present invention, D1 and D2 preferably satisfy the relationship D1≦0.9D2, more preferably D1≦0.8D2, D1≦0.7D2, D1≦0.6D2, D1≦0.55D2, or D1≦0.5D2. A method for measuring the average particle size of the inorganic filler will be described later. In another embodiment, the first resin composition layer may be substantially free of an inorganic filler. For example, when the non-volatile components in the first resin composition layer are taken as 100% by mass, the content of the inorganic filler may be 5% by mass or less, 4% by mass or less, 3% by mass or less, 2% by mass or less, 1% by mass or less, or 0.5% by mass or less. Alternatively, the first resin composition layer may be free of an inorganic filler.

[0027] In the multilayer resin sheet of the present invention, the layers other than the first resin composition layer are preferably thicker than the first resin composition layer, from the viewpoint of providing an insulating layer with better surface smoothness, reduced smears, and well-shaped via holes, even when a desmear treatment is performed after peeling off the support. Thus, in a preferred embodiment, when the thickness (μm) of the multilayer resin sheet is T and the thickness (μm) of the first resin composition layer is t, the relationship t<(T-t) holds. From the viewpoint of further enjoying the effects of the present invention, the above t and T preferably satisfy the relationship t≦0.2T, more preferably t≦0.15T, t≦0.1T, t≦0.08T, t≦0.06T, or t≦0.05T. Furthermore, from the viewpoint of providing an insulating layer having better surface smoothness, reduced smears, and well-shaped via holes even when desmearing is performed after peeling off the support, and further from the viewpoint of providing an insulating layer with little change in film thickness before and after desmearing, t and T preferably satisfy the relationship of 0.005T≦t, 0.01T≦t, or 0.02T≦t. In the multilayer resin sheet of the present invention, when the thickness (μm) of the resin composition layer that is the outermost layer on the side opposite to the first resin composition layer is defined as t', t' preferably satisfies the relationship of t'≧0.1(T−t), and more preferably satisfies the relationship of t'≧0.2(T−t), t'≧0.3(T−t), t'≧0.4(T−t), or t'≧0.5(T−t).

[0028] The thickness T of the multilayer resin sheet of the present invention varies depending on the application, and may be appropriately determined depending on the application. For example, from the viewpoint of thinning the printed wiring board, the thickness T of the multilayer resin sheet is preferably 200 μm or less, more preferably 150 μm or less, 120 μm or less, 100 μm or less, 80 μm or less, 60 μm or less, or 50 μm or less. The lower limit of the thickness T is not particularly limited, but can usually be 5 μm or more, 10 μm or more, etc.

[0029] The resin composition layers constituting the multilayer resin sheet of the present invention are described in detail below. Hereinafter, when it is preferable to use different blending components or blending amounts between the first resin composition layer and the other resin composition layers, this will be specified separately. Unless otherwise specified, the blending components and blending amounts of the first resin composition layer can be applied by replacing the term "resin composition layer" described below with "first resin composition layer," and the blending components and blending amounts of the layers other than the first resin composition layer can be applied by replacing the term "resin composition layer" described below with "layers other than the first resin composition layer." When the multilayer resin sheet of the present invention has a structure in which N resin composition layers (where N is an integer of 3 or more) are laminated, the blending amounts of the blending components in the layers other than the first resin composition layer refer to the blending amounts of each blending component relative to the total number of layers (N-1) other than the first resin composition layer, and the physical properties of the blending components in the layers other than the first resin composition layer refer to the average value of the physical properties of each blending component relative to the total number of layers (N-1) other than the first resin composition layer.

[0030] -Inorganic Filler- In the multilayer resin sheet of the present invention, the resin composition layer may contain an inorganic filler as described above.

[0031] Examples of inorganic filler materials include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum silicate, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium titanate zirconate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly preferred. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. Spherical silica is preferred. The inorganic filler may be used alone or in combination of two or more.

[0032] Commercially available inorganic fillers include, for example, "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", "YA010C", "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.; "UFP-30", "DAW-03", and "FB-105FD" manufactured by Denka Co., Ltd.; "Silfil NSS-3N", "Silfil NSS-4N", and "Silfil NSS-5N" manufactured by Tokuyama Corporation; "CellSpheres" and "MGH-005" manufactured by Taiheiyo Cement Corporation; and "Sfereek" and "BA-1" manufactured by JGC Catalysts and Chemicals Co., Ltd.

[0033] The average particle size of the inorganic filler is not particularly limited, but is preferably 10 μm or less, more preferably 5 μm or less, even more preferably 3 μm or less, 2 μm or less, 1 μm or less, 0.8 μm or less, or 0.7 μm or less. The lower limit of the average particle size is not particularly limited, but is preferably 0.01 μm or more, more preferably 0.05 μm or more, even more preferably 0.07 μm or more, 0.1 μm or more, or 0.2 μm or more. The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is created on a volume basis using a laser diffraction / scattering particle size distribution analyzer, and the median diameter is used as the average particle size. The measurement sample can be prepared by weighing 100 mg of inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing it ultrasonically for 10 minutes. The measurement sample was measured using a laser diffraction particle size distribution analyzer, with blue and red light source wavelengths used and a flow cell system to measure the volumetric particle size distribution of the inorganic filler, and the average particle size was calculated as the median diameter from the obtained particle size distribution. An example of a laser diffraction particle size distribution analyzer is the "LA-960" manufactured by Horiba, Ltd.

[0034] As described above, when the first resin composition layer contains an inorganic filler, it is preferable that D1 < D2, where D1 is the average particle size (μm) of the inorganic filler in the first resin composition layer and D2 is the average particle size (μm) of the inorganic filler in the layers excluding the first resin composition layer. The preferred relationship between D1 and D2 is as described above. In particular, from the viewpoint of being able to provide a cured product with even lower surface roughness and better smoothness after desmearing, even when desmearing is performed after peeling off the support, D1 is preferably 1 μm or less, more preferably 0.8 μm or less, 0.7 μm or less, or 0.6 μm or less, and even more preferably 0.5 μm or less, 0.4 μm or less, 0.3 μm or less, or 0.2 μm or less. The lower limit of D1 is as described above and can be, for example, 0.01 μm or more, 0.02 μm or more, etc.

[0035] The inorganic filler is preferably surface-treated with an appropriate surface treatment agent. By performing the surface treatment, the moisture resistance and dispersibility of the inorganic filler can be improved. Examples of the surface treatment agent include silane coupling agents such as vinyl silane coupling agents, epoxy silane coupling agents, styryl silane coupling agents, (meth)acrylic silane coupling agents, amino silane coupling agents, isocyanurate silane coupling agents, ureido silane coupling agents, mercapto silane coupling agents, isocyanate silane coupling agents, and acid anhydride silane coupling agents; non-silane coupling alkoxysilane compounds such as methyltrimethoxysilane and phenyltrimethoxysilane; and silazane compounds. The surface treatment agents may be used alone or in combination of two or more.

[0036] Examples of commercially available surface treatment agents include "KBM403" (3-glycidoxypropyltrimethoxysilane), "KBM803" (3-mercaptopropyltrimethoxysilane), "KBE903" (3-aminopropyltriethoxysilane), "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), and "SZ-31" (hexamethyldisilazane), all manufactured by Shin-Etsu Chemical Co., Ltd.

[0037] The degree of surface treatment with the surface treatment agent is preferably within a predetermined range from the viewpoint of improving the dispersibility of the inorganic filler. Specifically, 100 parts by mass of the inorganic filler is preferably surface-treated with 0.2 to 5 parts by mass of the surface treatment agent.

[0038] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of ​​the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of ​​the inorganic filler is 0.02 mg / m 2 More than 0.1 mg / m 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of preventing an increase in the melt viscosity of the resin composition or the melt viscosity in the form of a sheet, it is more preferable that the content be 1.0 mg / m 2 Preferably, 0.8 mg / m or less 2 More preferably, 0.5 mg / m or less 2 The following is even more preferable. The carbon amount per unit surface area of ​​the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the carbon amount per unit surface area of ​​the inorganic filler can be measured using a carbon analyzer. As the carbon analyzer, an "EMIA-320V" manufactured by Horiba, Ltd. or the like can be used.

[0039] In the multilayer resin sheet of the present invention, the content of inorganic filler in the resin composition layer may be determined depending on the properties required of the multilayer resin sheet, but from the viewpoint of easily adjusting the RD / RA ratio within a suitable range and from the viewpoint of realizing a cured product exhibiting an even lower linear thermal expansion coefficient and dielectric loss tangent, when the nonvolatile components in the resin composition layer are taken as 100% by mass, the content C2 of inorganic filler in the layers excluding the first resin composition layer is preferably 40% by mass or 45% by mass or more, more preferably 50% by mass or more, 55% by mass or more, or 60% by mass or more, and even more preferably 65% ​​by mass or more, 66% by mass or more, 68% by mass or more, 70% by mass or more, 72% by mass or more, or 74% by mass or more. The upper limit of the content C2 is as described above, but is preferably 80% by mass or less, 75% by mass or less, or 70% by mass or less.

[0040] In one embodiment, the content C1 (mass%) of the inorganic filler in the first resin composition layer and the content C2 (mass%) of the inorganic filler in the layers other than the first resin composition layer satisfy the relationship C1 < C2. When C1 and C2 satisfy the above relationship, it is preferable because it is easy to adjust the RD / RA ratio to a suitable range. The suitable range of C2 is as described above.

[0041] As described above, the first resin composition layer may be substantially free of inorganic fillers. For example, when the nonvolatile components in the first resin composition layer are taken as 100% by mass, the content C1 of inorganic fillers in the first resin composition layer may be 5% by mass or less, 4% by mass or less, 3% by mass or less, 2% by mass or less, 1% by mass or less, or 0.5% by mass or less. Alternatively, the first resin composition layer may be free of inorganic fillers.

[0042] -Thermosetting Component- In the multilayer resin sheet of the present invention, the resin composition layer preferably contains a thermosetting resin.

[0043] Examples of thermosetting resins include epoxy resins, benzocyclobutene resins, epoxy acrylate resins, urethane acrylate resins, urethane resins, cyanate resins, unsaturated polyester resins, melamine resins, silicone resins, etc. The thermosetting resins may be used alone or in combination of two or more.

[0044] Among these, it is preferable that the thermosetting resin contains an epoxy resin, from the viewpoint of providing an insulating layer having better surface smoothness, reduced smears, and well-shaped via holes even when a desmear treatment is performed after peeling off the support, and further from the viewpoint of providing an insulating layer with little change in film thickness before and after the desmear treatment.

[0045] Examples of epoxy resins include bisphenol-type epoxy resins, dicyclopentadiene-type epoxy resins, trisphenol-type epoxy resins, naphthol novolac-type epoxy resins, phenol novolac-type epoxy resins, tert-butyl-catechol-type epoxy resins, naphthalene-type epoxy resins, naphthol-type epoxy resins, anthracene-type epoxy resins, glycidylamine-type epoxy resins, glycidyl ester-type epoxy resins, cresol novolac-type epoxy resins, biphenyl-type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane-type epoxy resins, cyclohexanedimethanol-type epoxy resins, naphthylene ether-type epoxy resins, trimethylol-type epoxy resins, and tetraphenylethane-type epoxy resins. Bisphenol-type epoxy resins refer to epoxy resins having a bisphenol structure, such as bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, bisphenol S-type epoxy resins, and bisphenol AF-type epoxy resins. Biphenyl-type epoxy resin refers to an epoxy resin having a biphenyl structure, where the biphenyl structure may have a substituent such as an alkyl group, an alkoxy group, or an aryl group. Therefore, bixylenol-type epoxy resins and biphenylaralkyl-type epoxy resins are also included in the biphenyl-type epoxy resin. The epoxy resins may be used alone or in combination of two or more.

[0046] The epoxy resin is preferably an aromatic epoxy resin, which means an epoxy resin having an aromatic ring in its molecule.

[0047] The epoxy resin preferably has two or more epoxy groups in one molecule. When the non-volatile components of the epoxy resin are taken as 100% by mass, the proportion of the epoxy resin having two or more epoxy groups in one molecule is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more.

[0048] Epoxy resins include those that are liquid at a temperature of 20°C (hereinafter referred to as "liquid epoxy resins") and those that are solid at a temperature of 20°C (hereinafter referred to as "solid epoxy resins").

[0049] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.

[0050] Preferred liquid epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, naphthalene type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, phenol novolac type epoxy resins, alicyclic epoxy resins such as alicyclic epoxy resins having an ester skeleton, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, and epoxy resins having a butadiene structure.

[0051] Specific examples of liquid epoxy resins include "HP-4032", "HP-4032D", and "HP-4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "jER828EL", "825", and "Epicoat 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; and "630" and "630LSD" (p-aminophenol type epoxy resins, glycidyl ether type epoxy resins) manufactured by Mitsubishi Chemical Corporation. Examples of epoxy resins that can be used include "ZX1059" (a mixture of bisphenol A epoxy resin and bisphenol F epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "EX-721" (a glycidyl ester epoxy resin) manufactured by Nagase ChemteX Corporation; "Celloxide 2021P" (an alicyclic epoxy resin having an ester skeleton) manufactured by Daicel Corporation; "PB-3600" (an epoxy resin having a butadiene structure) manufactured by Daicel Corporation; and "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.

[0052] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferred, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferred.

[0053] Preferred solid epoxy resins include bixylenol-type epoxy resins, naphthalene-type epoxy resins, naphthalene-type tetrafunctional epoxy resins, cresol novolac-type epoxy resins, dicyclopentadiene-type epoxy resins, trisphenol-type epoxy resins, naphthol-type epoxy resins, biphenyl-type epoxy resins, naphthylene ether-type epoxy resins, anthracene-type epoxy resins, bisphenol A-type epoxy resins, bisphenol AF-type epoxy resins, and tetraphenylethane-type epoxy resins.

[0054] Specific examples of solid epoxy resins include "HP-4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200HH", "HP-7200H", and "HP-7200" (dicyclopentadiene epoxy resins) manufactured by DIC Corporation. DIC Corporation's "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", and "HP6000" (naphthylene ether type epoxy resins); Nippon Kayaku Co., Ltd.'s "EPPN-502H" (trisphenol type epoxy resin); Nippon Kayaku Co., Ltd.'s "NC-7000-L" (naphthol novolac type epoxy resin); Nippon Kayaku Co., Ltd.'s "NC-3000-H", "NC-3000", and "NC-300 0-L" and "NC-3100" (biphenyl-type epoxy resin); "ESN475V" (naphthol-type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN485" (naphthol novolac-type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YX4000", and "YL6121" (biphenyl-type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "YX4000HK" (bixylenol-type epoxy resin) manufactured by Mitsubishi Chemical Corporation. "YX8800" (anthracene-type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals Co., Ltd.; "YL7760" (bisphenol AF-type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "YL7800" (fluorene-type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "jER1010" (solid bisphenol A-type epoxy resin) manufactured by Mitsubishi Chemical Corporation; and "jER1031S" (tetraphenylethane-type epoxy resin) manufactured by Mitsubishi Chemical Corporation.

[0055] In the multilayer resin sheet of the present invention, the resin composition layer may contain only a liquid epoxy resin as the epoxy resin, only a solid epoxy resin, or a combination of a liquid epoxy resin and a solid epoxy resin. From the viewpoint of easily adjusting the RD / RA ratio within a suitable range, the resin composition layer preferably contains a solid epoxy resin. When a liquid epoxy resin and a solid epoxy resin are used in combination, the ratio by mass (liquid epoxy resin:solid epoxy resin) is preferably 1:0.5 to 1:50, more preferably 1:1 to 1:30, and even more preferably 1:2 to 1:20. From the viewpoint of easily adjusting the RD / RA ratio within a suitable range, the mass ratio X1 of the solid epoxy resin / liquid epoxy resin in the first resin composition layer is preferably higher than the mass ratio X2 of the solid epoxy resin / liquid epoxy resin in the layers other than the first resin composition layer, and for example, the difference (X1-X2) between the mass ratio X1 and the mass ratio X2 may be 1 or more, 2 or more, 3 or more, 4 or more, or 5 or more. The upper limit of the difference (X1-X2) may usually be 20 or less, 15 or less, 14 or less, 12 or less, or the like.

[0056] The epoxy equivalent of the epoxy resin is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., even more preferably 80 g / eq. to 2000 g / eq., and even more preferably 110 g / eq. to 1000 g / eq. The epoxy equivalent is the mass of an epoxy resin containing one equivalent of epoxy groups. This epoxy equivalent can be measured in accordance with JIS K7236.

[0057] The weight average molecular weight (Mw) of the epoxy resin is preferably 100 to 5000, more preferably 250 to 3000, and even more preferably 400 to 1500. The Mw of the epoxy resin can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).

[0058] From the viewpoint of easily adjusting the RD / RA ratio within a suitable range, providing an insulating layer with better surface smoothness, reduced smear, and well-shaped via holes, the content of the thermosetting resin in the resin composition layer is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 12% by mass or more, 14% by mass or more, or 15% by mass or more, when the resin component in the resin composition layer is 100% by mass. The upper limit of the content is not particularly limited and may be determined depending on the properties required of the resin composition, but may be, for example, 60% by mass or less, 50% by mass or less, 45% by mass or less, or 40% by mass or less.

[0059] In the present invention, the "resin component" of the resin composition layer refers to the solid components (non-volatile components) constituting the resin composition layer, excluding the inorganic filler described below.

[0060] In the multilayer resin sheet of the present invention, the resin composition layer may contain, in addition to the thermosetting resin and inorganic filler, one or more selected from a curing agent, a thermoplastic resin, a radical polymerizable resin, and a curing accelerator.

[0061] - Curing Agent - In the multilayer resin sheet of the present invention, the resin composition layer preferably contains a curing agent, which generally has the function of reacting with the thermosetting resin to cure the resin composition layer.

[0062] Examples of the curing agent include active ester curing agents, phenol curing agents, naphthol curing agents, acid anhydride curing agents, cyanate ester curing agents, carbodiimide curing agents, amine curing agents, etc. The curing agents may be used alone or in combination of two or more.

[0063] In particular, from the viewpoint of obtaining an insulating layer having better surface smoothness, reduced smear, and well-shaped via holes even when a desmear treatment is performed after peeling off the support, the curing agent preferably contains one or more selected from the group consisting of an active ester-based curing agent, a phenol-based curing agent, and a naphthol-based curing agent, and from the viewpoint of easily adjusting the RD / RA ratio within a suitable range and obtaining an insulating layer having better surface smoothness, reduced smear, and well-shaped via holes, it is preferable that the curing agent contains an active ester-based curing agent. Thus, in one embodiment, the curing agent contains one or more selected from the group consisting of an active ester-based curing agent, a phenol-based curing agent, and a naphthol-based curing agent, and more preferably contains an active ester-based curing agent.

[0064] As the active ester curing agent, a compound having one or more active ester groups per molecule can be used. Among them, preferred active ester curing agents are compounds having two or more highly reactive ester groups per molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds. The active ester curing agent is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, active ester curing agents derived from carboxylic acid compounds are preferred, active ester curing agents obtained from a carboxylic acid compound and a hydroxy compound are more preferred, and active ester curing agents obtained from a carboxylic acid compound and an aromatic hydroxy compound are even more preferred.

[0065] The carboxylic acid compound may be either an aromatic carboxylic acid compound or an aliphatic carboxylic acid, and examples thereof include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid.

[0066] Examples of aromatic hydroxy compounds include (i) polyaddition products of unsaturated aliphatic cyclic compounds containing two double bonds per molecule with phenols, (ii) various bisphenol compounds, (iii) aromatic polyols having two or more hydroxy groups bonded to a carbon atom on an aromatic ring, and (iv) aromatic monools having one hydroxy group bonded to a carbon atom on an aromatic ring. Examples of polyaddition products of unsaturated aliphatic cyclic compounds with phenols include polyaddition products of unsaturated aliphatic cyclic compounds such as dicyclopentadiene, tetrahydroindene, norbornadiene, limonene, and vinylcyclohexene with phenols that may have a substituent (e.g., phenol, cresol, xylenol, ethylphenol, propylphenol, vinylphenol, allylphenol, phenylphenol, benzylphenol, and halophenols), and specific examples thereof include dicyclopentadiene-phenol polyaddition products. Examples of bisphenol compounds include bisphenol A, bisphenol F, bisphenol AF, bisphenol AP, bisphenol B, bisphenol BP, bisphenol C, and bisphenol M. Examples of aromatic polyols having two or more hydroxy groups bonded to carbon atoms on an aromatic ring include hydroquinone, resorcinol, catechol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucinol, benzenetriol, and phenol novolak. Examples of aromatic monools having one hydroxy group bonded to a carbon atom on an aromatic ring include phenol, cresol, xylenol, ethylphenol, propylphenol, vinylphenol, allylphenol, phenylphenol, benzylphenol, halophenols, naphthol, methylnaphthol, dimethylnaphthol, ethylnaphthol, propylnaphthol, vinylnaphthol, allylnaphthol, phenylnaphthol, benzylnaphthol, and halonaphthol.

[0067] Specific preferred examples of the active ester curing agent include active ester compounds containing a dicyclopentadiene-type diphenol structure, active ester compounds containing a naphthalene structure, active ester compounds containing an acetylated product of phenol novolac, and active ester compounds containing a benzoylated product of phenol novolac. Among these, active ester compounds containing a naphthalene structure and active ester compounds containing a dicyclopentadiene-type diphenol structure are more preferred. The "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentalene-phenylene.

[0068] Commercially available active ester curing agents include active ester resins containing a dicyclopentadiene-type diphenol structure such as "EXB-9451", "EXB-9460", "EXB-9460S", "HPC-8000-65T", "HPC-8000H-65TM", and "HPC-8000L-65TM" (manufactured by DIC Corporation); active ester resins containing a naphthalene structure such as "EXB-8100L-65T", "EXB-8150-60T", "EXB-8150-62T", "EXB-9416-70BK", "HPC-8150-60T", and "HPC-8150-62T"; Examples of such active ester resins include "HP-B-8151-62T" and "HP-C-8151-62T" (manufactured by DIC Corporation); "EXB9401" (manufactured by DIC Corporation) as a phosphorus-containing active ester resin; "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester resin which is an acetylated product of phenol novolac; "YLH1026," "YLH1030," and "YLH1048" (manufactured by Mitsubishi Chemical Corporation) as active ester resins which are benzoylated products of phenol novolac; and "PC1300-02-65MA" (manufactured by Air Water Inc.) as an active ester resin containing a styryl group and a naphthalene structure.

[0069] As the phenol-based curing agent and naphthol-based curing agent, those having a novolac structure are preferred from the viewpoint of heat resistance and water resistance. Furthermore, from the viewpoint of adhesion to the conductor layer, nitrogen-containing phenol-based curing agents and nitrogen-containing naphthol-based curing agents are preferred, and triazine skeleton-containing phenol-based curing agents and triazine skeleton-containing naphthol-based curing agents are more preferred.

[0070] Specific examples of phenol-based curing agents and naphthol-based curing agents include "MEH-7700", "MEH-7810", "MEH-7851", and "MEH-8000H" manufactured by Meiwa Chemical Industry Co., Ltd.; "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd.; and "SN-170", "SN-180", "SN-190", "SN-475", "SN-485", "SN-495", "SN-495V", and "SN-37" manufactured by Nippon Steel Chemical & Material Co., Ltd. 5" and "SN-395" manufactured by DIC Corporation; "TD-2090", "TD-2090-60M", "LA-7052", "LA-7054", "LA-1356", "LA-3018", "LA-3018-50P", "EXB-9500", "HPC-9500", "KA-1160", "KA-1163", and "KA-1165" manufactured by Gun-ei Chemical Co., Ltd.; and "GDP-6115L", "GDP-6115H", and "ELPC75" manufactured by Gun-ei Chemical Co., Ltd.

[0071] Examples of acid anhydride curing agents include curing agents having one or more acid anhydride groups in one molecule. Specific examples of acid anhydride curing agents include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, and benzophenonetetracarboxylic dianhydride. Examples of suitable acid anhydrides include polymeric acid anhydrides such as styrene-maleic acid resins obtained by copolymerizing styrene and maleic acid, ethylene glycol bis(anhydrotrimellitate), styrene anhydride, bis(trimethylsilyl)propanol ...

[0072] Examples of cyanate ester curing agents include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanatephenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanatephenyl-1-(methylethylidene))benzene, bis(4-cyanatephenyl)thioether, and bis(4-cyanatephenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially triazine converted. Specific examples of cyanate ester curing agents include "PT30" and "PT60" (phenol novolac type multifunctional cyanate ester resins), "ULL-950S" (multifunctional cyanate ester resin), "BA230" and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been triazinated to form a trimer), all of which are manufactured by Arxada.

[0073] Specific examples of carbodiimide curing agents include Carbodilite (registered trademark) V-03 (carbodiimide group equivalent: 216 g / eq.), V-05 (carbodiimide group equivalent: 262 g / eq.), and V-07 (carbodiimide group equivalent: 200 g / eq.), all manufactured by Nisshinbo Chemical Inc.; and V-09 (carbodiimide group equivalent: 200 g / eq.); and Stabaxol (registered trademark) P (carbodiimide group equivalent: 302 g / eq.) manufactured by Lanxess AG.

[0074] Examples of the amine-based curing agent include curing agents having one or more amino groups in one molecule, such as aliphatic amines, polyether amines, alicyclic amines, and aromatic amines. Specific examples of the amine-based curing agent include 4,4'-methylenebis(2,6-dimethylaniline), diphenyldiaminosulfone, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenyl ether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, and 2,2-bis(3-amino-4-hydroxybenzoyl)methylpropional. bis(4-aminophenoxy)biphenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, and the like. Commercially available amine-based curing agents may be used, and examples thereof include "KAYABOND C-200S," "KAYABOND C-100," "KAYAHARD A-A," "KAYAHARD A-B," and "KAYAHARD A-S" manufactured by Nippon Kayaku Co., Ltd., and "Epicure W" manufactured by Mitsubishi Chemical Corporation.

[0075] Even when a desmear treatment is performed after peeling off the support, from the viewpoint of providing an insulating layer with better surface smoothness, reduced smears, and well-shaped via holes, the content of the curing agent in the resin composition is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, 35% by mass or more, or 40% by mass or more, based on 100% by mass of the resin component in the resin composition. The upper limit of the content is not particularly limited and may be determined depending on the properties required of the resin composition, but may be, for example, 80% by mass or less, 75% by mass or less, or 70% by mass or less.

[0076] As mentioned above, the curing agent preferably contains an active ester curing agent, from the viewpoints of easily adjusting the RD / RA ratio within a suitable range, providing an insulating layer with improved surface smoothness, reduced smear, and well-shaped via holes. In the multilayer resin sheet of the present invention, when the resin composition layer contains an active ester curing agent as the curing agent, the content of the active ester curing agent in the curing agent is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, 75% by mass or more, or 80% by mass or more, based on 100% by mass of the non-volatile components of the curing agent, from the viewpoints of being able to further enjoy the effects of the present invention and obtaining a cured product exhibiting particularly excellent dielectric properties. The upper limit of the content of the active ester curing agent in the curing agent is not particularly limited, and may be 100% by mass, but may also be, for example, 95% by mass or less, 90% by mass or less, etc.

[0077] When the resin composition layer in the multilayer resin sheet of the present invention contains an active ester curing agent as a curing agent, the mass ratio of the active ester curing agent to the thermosetting resin (active ester curing agent / thermosetting resin) is preferably 0.5 or more, more preferably 0.6 or more, even more preferably 0.8 or more, 1 or more, 1.1 or more, 1.2 or more, 1.3 or more, 1.4 or more, or 1.5 or more, from the viewpoint of being able to further enjoy the effects of the present invention and exhibiting particularly excellent dielectric properties. The upper limit of this mass ratio (active ester curing agent / thermosetting resin) may be, for example, 5 or less, 4.5 or less, or 4 or less. In particular, from the viewpoint of easily adjusting the etching rate RA to a suitable range and thus easily adjusting the RD / RA ratio to a suitable range, the mass ratio (active ester curing agent / thermosetting resin) in the first resin composition layer is preferably 1 or more, more preferably 1.2 or more or 1.4 or more, even more preferably 1.5 or more, 16 or more, 1.8 or more, or 2 or more.

[0078] -Thermoplastic Resin- In the multilayer resin sheet of the present invention, the resin composition layer may contain a thermoplastic resin.

[0079] Examples of thermoplastic resins include phenoxy resins, polyimide resins, polyvinyl acetal resins, acrylic resins, polyolefin resins, polybutadiene resins, polyamideimide resins, polysulfone resins, polyethersulfone resins, polyphenylene ether resins, polyetherimide resins, polycarbonate resins, polyetheretherketone resins, and polyester resins, and among these, resins selected from phenoxy resins, polyimide resins, acrylic resins, polyphenylene ether resins, and polycarbonate resins are preferred. The thermoplastic resins may be used alone or in combination of two or more.

[0080] --Phenoxy Resin-- Examples of phenoxy resins include phenoxy resins having one or more skeletons selected from the group consisting of a bisphenol A skeleton, a bisphenol F skeleton, a bisphenol S skeleton, a bisphenolacetophenone skeleton, a novolac skeleton, a biphenyl skeleton, a fluorene skeleton, a dicyclopentadiene skeleton, a norbornene skeleton, a naphthalene skeleton, an anthracene skeleton, an adamantane skeleton, a terpene skeleton, and a trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group. One type of phenoxy resin may be used alone, or two or more types may be used in combination. Specific examples of phenoxy resins include "1256" and "4250" (both phenoxy resins containing a bisphenol A skeleton), "YX8100" (phenoxy resin containing a bisphenol S skeleton), and "YX6954" (phenoxy resin containing a bisphenol acetophenone skeleton) manufactured by Mitsubishi Chemical Corporation; "FX280" and "FX293" manufactured by Nippon Steel Chemical & Material Co., Ltd.; and "YX7200B35," "YX7500BH30," "YX6954BH30," "YX7553," "YX7553BH30," "YL7769BH30," "YL6794," "YL7213," "YL7290," and "YL7482" manufactured by Mitsubishi Chemical Corporation.

[0081] --Polyimide Resin-- A resin having an imide structure can be used as the polyimide resin. Polyimide resins can generally be obtained by the imidization reaction between a diamine compound and an acid anhydride, or the imidization reaction between a diisocyanate compound and an acid anhydride. Specific examples of polyimide resins include linear polyimides obtained by reacting bifunctional hydroxyl-terminated polybutadiene, a diisocyanate compound, and a tetrabasic acid anhydride (polyimides described in JP 2006-37083 A), and modified polyimides such as polysiloxane skeleton-containing polyimides (polyimides described in JP 2002-12667 A and JP 2000-319386 A). Commercially available polyimide resins may also be used, such as "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd.

[0082] Particularly preferred examples of polyimide resins are shown below. In a preferred embodiment, the polyimide resin contains a structural unit represented by the following formula (1) (hereinafter also referred to as "structural unit (1)"). The number of structural units (1) contained per molecule of the polyimide resin is 1 or more, and is not particularly limited, but may be 100 or less, 50 or less, or 30 or less.

[0083] [In formula (1), R 1 is a tetravalent group represented by the following formula (1-1), 2 is a divalent group represented by the following formula (1-2).

[0084] (In formula (1-1), Ar 11 , Ar 12 , Ar 13 and Ar 14 each independently represents an aromatic ring which may have a substituent; L 11 , L 12 and L 13 each independently represents a divalent linking group, and nc1 represents an integer of 0 or more.

[0085] (In formula (1-2), Ar 21 , Ar 22 , Ar 23 and Ar 24 each independently represents an aromatic ring which may have a substituent; 21 , L 22 and L 23 each independently represents a divalent linking group, and nc2 represents an integer of 1 or greater.

[0086] In formula (1-1), Ar 11 , Ar 12 , Ar 13 and Ar 14 The aromatic ring represented by (hereinafter also referred to as "aromatic ring C") is preferably an aromatic ring having 6 to 100 carbon atoms, more preferably 6 to 50 carbon atoms, even more preferably 6 to 100 carbon atoms, and even more preferably 6 to 50 carbon atoms. 11 , Ar 12 , Ar13 and Ar 14 are each independently an aromatic carbocyclic ring having 6 to 14 carbon atoms which may have a substituent. Here, the term "aromatic ring" as used herein means a ring that conforms to Huckel's rule, in which the number of electrons contained in the π-electron system of the ring is 4n+2 (n is a natural number), and includes monocyclic aromatic rings and fused aromatic rings in which two or more monocyclic aromatic rings are fused together. The aromatic ring may be a carbocyclic ring or a heterocyclic ring. Examples of the aromatic ring include monocyclic aromatic rings such as a benzene ring, a furan ring, a thiophene ring, a pyrrole ring, a pyrazole ring, an oxazole ring, an isoxazole ring, a thiazole ring, an imidazole ring, a pyridine ring, a pyridazine ring, a pyrimidine ring, and a pyrazine ring; fused rings in which two or more monocyclic aromatic rings are fused, such as a naphthalene ring, an anthracene ring, a benzofuran ring, an isobenzofuran ring, an indole ring, an isoindole ring, a benzothiophene ring, a benzimidazole ring, an indazole ring, a benzoxazole ring, a benzisoxazole ring, a benzothiazole ring, a quinoline ring, an isoquinoline ring, a quinoxaline ring, an acridine ring, a quinazoline ring, a cinnoline ring, and a phthalazine ring; and fused rings in which one or more monocyclic aromatic rings are fused to one or more monocyclic non-aromatic rings, such as an indane ring, a fluorene ring, and a tetralin ring. Of these, aromatic carbon rings having 6 to 14 carbon atoms are preferred, with benzene rings being more preferred.

[0087] In formula (1-1), Ar 11 , Ar 12 , Ar 13 and Ar 14 When represents an aromatic ring having a substituent, the number of the substituents is not limited. Such substituents (hereinafter also referred to as "substituent S") include, independently of one another, a halogen atom, an alkyl group, a cycloalkyl group, an alkoxy group, a cycloalkyloxy group, an aryl group, an aryloxy group, an arylalkyl group, an arylalkoxy group, a monovalent heterocyclic group, an alkylidene group, an amino group, a silyl group, an acyl group, an acyloxy group, a carboxy group, a sulfo group, a cyano group, a nitro group, a hydroxy group, a mercapto group, and an oxo group.

[0088] In formula (1-1), L 11 , L 12 and L13 The divalent linking group represented by is preferably a divalent group consisting of one or more (for example, 1 to 3000, 1 to 1000, 1 to 100, or 1 to 50) skeletal atoms selected from carbon atoms, oxygen atoms, nitrogen atoms, sulfur atoms, and silicon atoms. Examples of the divalent linking group include -SO 2 -, -CO-, -COO-, -O-, -S-, -O-C 6 H 4 -O- (wherein -C 6 H 4 - represents a phenylene group), -O-C 6 H 4 -C(CH 3 ) 2 -C 6 H 4 -O-, -COO-(CH 2 ) q -OCO- (wherein q represents an integer of 1 to 20), -COO-H 2 C-HC(-OC(=O)-CH 3 )-CH 2 -OCO-, an alkylene group, an alkenylene group, an alkynylene group, an arylene group, a heteroarylene group, -C(=O)-, -C(=O)-O-, -NR 0 - (where R 0 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms; and —C(═O)—NR 0 -. The number of carbon atoms in the alkylene group is preferably 1 to 10, more preferably 1 to 6, even more preferably 1 to 5 or 1 to 4. The number of carbon atoms in the alkenylene group is preferably 2 to 10, more preferably 2 to 6, even more preferably 2 to 5. The number of carbon atoms in the arylene group is preferably 6 to 20, more preferably 6 to 10, and the number of carbon atoms in the heteroarylene group is preferably 2 to 20, more preferably 3 to 10, 4 to 10, or 5 to 10. The above-mentioned alkyl group, alkylene group, alkenylene group, alkynylene group, arylene group, and heteroarylene group may further have a substituent. Examples of the substituent include the above-mentioned substituent S. L 11 , L 12 and L 13 Preferably, the divalent linking group represented by does not contain an aromatic ring.11 and a divalent linking group represented by 13 and the divalent linking group represented by 11 and a divalent linking group represented by 12 In a preferred embodiment, in formula (1-1), L 11 and L 13 is -O-, and L 12 is an alkylene group which may have a substituent, and in a more preferred embodiment, in formula (1-1), Ar 11 , Ar 12 , Ar 13 and Ar 14 are each independently an aromatic carbocyclic ring having 6 to 14 carbon atoms which may have a substituent, and L 11 and L 13 is -O-, and L 12 In a more preferred embodiment, in formula (1-1), L 11 and L 13 is -O-, and L 12 is a dimethylmethylene group.

[0089] In formula (1-2), Ar 21 , Ar 22 , Ar 23 and Ar 24 Examples of the aromatic ring represented by and the substituent that the aromatic ring may have are the same as those of the aromatic ring C and the substituent S, respectively. 21 , Ar 22 , Ar 23 and Ar 24 are each independently an aromatic carbocyclic ring having 6 to 14 carbon atoms which may have a substituent. 21 and L 23 is -O-, and L 22 is an alkylene group which may have a substituent, and in a more preferred embodiment, in formula (1-2), Ar 21 , Ar 22 , Ar 23 and Ar 24are each independently an aromatic carbocyclic ring having 6 to 14 carbon atoms which may have a substituent, and L 21 and L 23 is -O-, and L 22 In a more preferred embodiment, in formula (1-2), L 21 and L 23 is -O-, and L 22 is a dimethylmethylene group.

[0090] In a particularly preferred embodiment, in formula (1-1), Ar 11 , Ar 12 , Ar 13 and Ar 14 are each independently an aromatic carbocyclic ring having 6 to 14 carbon atoms which may have a substituent, and in formula (1-2), Ar 21 , Ar 22 , Ar 23 and Ar 24 are each independently an aromatic carbocyclic ring having 6 to 14 carbon atoms which may have a substituent. 11 and L 13 is -O-, and L 12 is an alkylene group which may have a substituent, and in formula (1-2), L 21 and L 23 is -O-, and L 22 is an alkylene group which may have a substituent.

[0091] In formula (1-1), nc1 preferably represents an integer of 1 or greater. The upper limit of the integer represented by nc1 is not particularly limited, but may be, for example, 50, 40, 30, or 20.

[0092] In formula (1-2), nc2 preferably represents an integer of 2 or greater. The upper limit of the integer represented by nc2 is not particularly limited, but may be, for example, 60, 50, 40, or 30.

[0093] The structural unit (1) can be obtained, for example, by a known method for producing a polyimide resin, typically by imidizing a monomer composition containing a tetracarboxylic dianhydride and a diamine compound through polymerization, or by imidizing a monomer composition containing a tetracarboxylic dianhydride and a diisocyanate compound through polymerization. Note that the polyimide resin may partially contain a polyamic acid structure that may be generated during the imidization process.

[0094] The structural unit (1) may be obtained, for example, by reacting 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (a compound represented by the following formula (I); hereinafter, also referred to as "BPADA") with 4,4'-[1,4-phenylenebis[(1-methylethylidene)-4,1-phenyleneoxy]]bisbenzenamine (a compound represented by the following formula (II); hereinafter, also referred to as "BPPAN"). That is, R 1 is a skeleton derived from BPADA, and R 2 is a backbone derived from BPPAN.

[0095]

[0096]

[0097] The polyimide resin may further include a structural unit represented by the following formula (2) (hereinafter also referred to as "structural unit (2)"). Accordingly, in one embodiment, the polyimide resin further includes a structural unit represented by the following formula (2). The number of structural units (2) contained per molecule of the polyimide resin is 0 or more, and is not particularly limited, but may be 100 or less, 50 or less, or 30 or less.

[0098] (In formula (2), R 3 represents a tetravalent aliphatic group which may have a substituent or a tetravalent aromatic group which may have a substituent, R 4 represents a divalent aliphatic group which may have a substituent or a divalent aromatic group which may have a substituent, provided that R 3 is R 1 If it is the same as4 is R 2 Unlike R 4 is R 2 If it is the same as 3 is R 1 It is different from.)

[0099] In formula (2), R 3 The tetravalent aliphatic group represented by R contains at least a carbon atom, and is preferably a tetravalent group consisting of one or more (e.g., 1 to 3000, 1 to 1000, 1 to 100, or 1 to 50) skeletal atoms selected from carbon atoms, oxygen atoms, nitrogen atoms, sulfur atoms, and silicon atoms. 3 The tetravalent aliphatic group represented by is more preferably a tetravalent aliphatic group having 1 to 100 carbon atoms, and even more preferably 1 to 50 carbon atoms. 3 When represents a tetravalent aliphatic group having a substituent, examples of the substituent are the same as the examples of the substituent S.

[0100] In formula (2), R 3 The tetravalent aromatic group represented by is preferably a tetravalent aromatic group having 6 to 100 carbon atoms, more preferably 6 to 50 carbon atoms. The aromatic group contains at least an aromatic ring. Examples of the aromatic ring contained in the aromatic group include Ar 11 , Ar 12 , Ar 13 and Ar 14 In formula (2), R 3 When represents a tetravalent aromatic group having a substituent, examples of the substituent are the same as the examples of the substituent S.

[0101] R 3 Examples of the tetravalent aromatic group represented by the formula (I) include a group obtained by removing two acid anhydride groups from a tetracarboxylic acid dianhydride having an aromatic group which may have a substituent. Specific examples of the tetracarboxylic acid dianhydride having an aromatic group which may have a substituent include BPADA, pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, 4,4'-oxydiphthalic anhydride, 3,3',4,4'-benzophenonetetracarboxylic acid dianhydride, and 3,3',4,4'-diphenylsulfonetetracarboxylic acid dianhydride.

[0102] In formula (2), R 4 The divalent aliphatic group represented by formula (2) contains at least a carbon atom, and is preferably a divalent group consisting of one or more (e.g., 1 to 3000, 1 to 1000, 1 to 100, 1 to 50) skeletal atoms selected from carbon atoms, oxygen atoms, nitrogen atoms, sulfur atoms, and silicon atoms. 4 The divalent aliphatic group represented by is more preferably a divalent aliphatic group having 1 to 100 carbon atoms, and even more preferably 1 to 50 carbon atoms. 4 When R represents a divalent aliphatic group having a substituent, examples of the substituent are the same as the examples of the substituent S, for example, an alkyl group having 1 to 6 carbon atoms. 4 is a divalent aliphatic group which may have a substituent, one of which is an alkyl group having 1 to 6 carbon atoms. 4 is a divalent aliphatic group which may have a substituent, and is a divalent group obtained by removing two amino groups from isophoronediamine.

[0103] R 4 represents a divalent aliphatic group which may have a substituent, it may be a group obtained by removing two amino groups from a diamine compound having a linear aliphatic group which may have a substituent, selected from 1,2-diaminoethane, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, and 1,12-dodecanediamine.

[0104] R 4 represents a divalent aliphatic group which may have a substituent, it may be a group obtained by removing two amino groups from a diamine compound which has a branched aliphatic group which may have a substituent selected from 1,2-diaminopropane, 1,2-diamino-2-methylpropane, 1,3-diamino-2-methylpropane, 1,3-diamino-2,2-dimethylpropane, 1,3-diaminopentane, and 1,5-diamino-2-methylpentane.

[0105] R 4represents a divalent aliphatic group which may have a substituent, examples thereof include 5-amino-1,3,3-trimethylcyclohexanemethylamine (isophoronediamine), 1,4-diaminocyclohexane, 1,3-diaminocyclohexane, 1,4-cyclohexanebis(methylamine), 1,3-cyclohexanebis(methylamine), 4,4'-diaminodicyclohexylmethane, bis(4-amino-3-methylcyclohexyl)methane, 3(4),8(9)-bis(aminomethyl)tricyclo[5.2.1.0 2,6 ]decane, 2,5(6)-bis(aminomethyl)bicyclo[2.2.1]heptane, 1,3-diaminoadamantane, 3,3'-diamino-1,1'-biadamantyl, and 1,6-diaminoadamantane, from which two amino groups have been removed. These diamine compounds are characterized in that the aliphatic group contains an alicyclic carbon ring.

[0106] In formula (2), R 4 The divalent aromatic group represented by is preferably a divalent aromatic group having 6 to 100 carbon atoms, more preferably 6 to 50 carbon atoms. The aromatic group contains at least an aromatic ring. Examples of the aromatic ring contained in the aromatic group are the same as the examples of the aromatic ring C. In formula (2), R 4 When represents a divalent aromatic group having a substituent, examples of the substituent are the same as the examples of the substituent S.

[0107] R 4 represents a divalent aromatic group which may have a substituent, it may be a group obtained by removing two amino groups from a diamine compound having an aromatic group which may have a substituent, selected from 4,4'-diaminodiphenyl ether, 1,4-phenylenediamine, and 2,2-bis[4-(4-aminophenoxy)phenyl]propane.

[0108] However, R 3 is R 1 If it is the same as 4 is R 2 Unlike R 4 is R 2 If it is the same as 3 is R 1In one embodiment, R 3 is R 1 is the same as

[0109] The structural unit (2) can be obtained, for example, by a known method for producing a polyimide resin. For example, the structural unit (2) can be obtained by reacting BPADA with isophoronediamine. That is, the R 3 is a skeleton derived from BPADA, and R 4 is a skeleton derived from isophoronediamine. 3 is R 1 If R is the same as 3 and R 1 is a skeleton derived from BPADA.

[0110] The terminal structure of the polyimide resin is not particularly limited. For example, the terminal structure of the polyimide resin may be an acid anhydride group, a carboxyl group, or an amino group derived from the raw material compound (e.g., an acid such as BPADA, or an amine compound such as BPPAN). When the raw material compound further contains maleic anhydride, the terminal structure of the polyimide resin may be a maleimide group.

[0111] The glass transition temperature Tg (°C) of the polyimide resin is preferably 140°C or higher, more preferably 145°C or higher, and even more preferably 150°C or higher, 160°C or higher, or 170°C or higher. There is no particular upper limit, but it can be set to 300°C or lower, for example. The glass transition temperature Tg (°C) of the polyimide resin can be measured by thermomechanical analysis (TMA).

[0112] The content of the structural unit (1) in the polyimide resin is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, 30% by mass or more, or 40% by mass or more. The upper limit of the content can be, for example, 98% by mass or less, 95% by mass or less, 90% by mass or less, or 85% by mass or less. Here, the content (mass percentage) of the structural unit (1) can be calculated from the ratio of the amounts (parts by mass) of each material used in the synthesis of the polyimide resin. Alternatively, the molecular weight of the polyimide resin and the formula weight of the structural unit (1) can be determined, and the content can be calculated as the ratio of the formula weight of the structural unit (1) to the molecular weight. When the polyimide resin is a polymer, the content of the structural unit (1) estimated from the degree of polymerization preferably falls within the above range.

[0113] When the polyimide resin further contains the structural unit (2), the content of the structural unit (2) may be 0% by mass (i.e., no structural unit (2) is contained), and there is no upper limit as long as the effects of the present invention are not impaired. The content of the structural unit (2) in the polyimide resin may be, for example, 1% by mass or more, 5% by mass or more, 10% by mass or more, 20% by mass or more, or 30% by mass or more, and 95% by mass or less, 90% by mass or less, 80% by mass or less, 70% by mass or less, or 60% by mass or less. Here, the content of the structural unit (2) is calculated in the same manner as the content of the structural unit (1).

[0114] The weight average molecular weight (Mw) of the polyimide resin is 1,000 or more, preferably 1.00 to 10,000, and more preferably 1,000 to 5,000. The weight average molecular weight of the resin can be measured by gel permeation chromatography (GPC) as a polystyrene-equivalent value.

[0115] --Polyvinyl acetal resin-- Examples of polyvinyl acetal resins include polyvinyl formal resins and polyvinyl butyral resins, with polyvinyl butyral resins being preferred. Specific examples of polyvinyl acetal resins include the S-LEC BH series, BX series (e.g., BX-5Z), KS series (e.g., KS-1), BL series, and BM series, all manufactured by Sekisui Chemical Co., Ltd.

[0116] Acrylic Resin: The term "acrylic resin" refers to a polymer obtained by polymerizing a monomer component containing a (meth)acrylic acid ester monomer. The monomer components constituting the acrylic resin may contain, in addition to the (meth)acrylic acid ester monomer, a (meth)acrylamide monomer, a styrene monomer, a functional group-containing monomer, or the like as copolymerization components. Specific examples of acrylic resins include "ARUFON UP-1000", "ARUFON UP-1010", "ARUFON UP-1020", "ARUFON UP-1021", "ARUFON UP-1061", "ARUFON UP-1080", "ARUFON UP-1110", "ARUFON UP-1170", "ARUFON UP-1190", "ARUFON UP-1500", "ARUFON UH-2000", "ARUFON UH-2041", "ARUFON UH-2190", "ARUFON UHE-2012", "ARUFON UC-3510", and "ARUFON UC-3510" manufactured by Toagosei Co., Ltd. Examples of such compounds include "ARUFON UG-4010," "ARUFON US-6100," and "ARUFON US-6170." These compounds may be used alone or in combination of two or more.

[0117] --Polyolefin Resin-- Examples of polyolefin resins include ethylene copolymer resins such as low-density polyethylene, very low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-methyl acrylate copolymer; and polyolefin elastomers such as polypropylene and ethylene-propylene block copolymer.

[0118] --Polybutadiene Resin-- Examples of polybutadiene resins include hydrogenated polybutadiene skeleton-containing resins, hydroxy group-containing polybutadiene resins, phenolic hydroxy group-containing polybutadiene resins, carboxy group-containing polybutadiene resins, acid anhydride group-containing polybutadiene resins, epoxy group-containing polybutadiene resins, isocyanate group-containing polybutadiene resins, urethane group-containing polybutadiene resins, and polyphenylene ether-polybutadiene resins.

[0119] --Polyamide-imide Resin-- Specific examples of polyamide-imide resins include "Vylomax HR11NN" and "Vylomax HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamide-imide resins also include modified polyamide-imides such as "KS9100" and "KS9300" (polysiloxane skeleton-containing polyamide-imides) manufactured by Resonac Corporation.

[0120] --Polyethersulfone Resin-- Specific examples of polyethersulfone resins include "PES5003P" manufactured by Sumitomo Chemical Co., Ltd.

[0121] --Polysulfone Resin-- Specific examples of polysulfone resins include polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers.

[0122] --Polyphenylene Ether Resin-- A specific example of a polyphenylene ether resin is "Noryl (registered trademark) SA90" manufactured by SABIC, etc. A specific example of a polyetherimide resin is "Ultem" manufactured by GE, etc.

[0123] --Polycarbonate Resin-- Examples of polycarbonate resins include hydroxy group-containing carbonate resins, phenolic hydroxy group-containing carbonate resins, carboxy group-containing carbonate resins, acid anhydride group-containing carbonate resins, isocyanate group-containing carbonate resins, and urethane group-containing carbonate resins. Specific examples of polycarbonate resins include "FPC0220" manufactured by Mitsubishi Gas Chemical Company, Inc., "T6002" and "T6001" (polycarbonate diols) manufactured by Asahi Kasei Corporation, and "C-1090," "C-2090," and "C-3090" (polycarbonate diols) manufactured by Kuraray Co., Ltd. Specific examples of polyether ether ketone resins include "Sumiploy K" manufactured by Sumitomo Chemical Co., Ltd. Examples of polyester resins include polyethylene terephthalate resins.

[0124] Unless otherwise specified, the weight average molecular weight of the thermoplastic resin is preferably 5,000 or more, more preferably 8,000 or more, even more preferably 10,000 or more, 15,000 or more, or 20,000 or more, and is preferably 200,000 or less, more preferably 150,000 or less, or 100,000 or less, even more preferably 80,000 or less, or 60,000 or less. The weight average molecular weight of the thermoplastic resin can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).

[0125] In the multilayer resin sheet of the present invention, when the resin composition layer contains a thermoplastic resin, the content of the thermoplastic resin in the resin composition layer is preferably 0.1 mass % or more, 0.3 mass % or more, or 0.5 mass % or more, when the resin component in the resin composition layer is taken as 100 mass %, from the viewpoints of easily adjusting the RD / RA ratio within a suitable range, providing an insulating layer with better surface smoothness, reduced smear, and well-shaped via holes. The upper limit of the thermoplastic resin content is not particularly limited, but is preferably 10 mass % or less, more preferably 8 mass % or less, and even more preferably 6 mass % or less or 5 mass % or less.

[0126] -Radical Polymerizable Resin- In the multilayer resin sheet of the present invention, the resin composition layer may contain a radical polymerizable resin.

[0127] The type of radical polymerizable resin is not particularly limited as long as it has one or more (preferably two or more) radical polymerizable unsaturated groups in one molecule. Examples of the radical polymerizable resin include resins having one or more radical polymerizable unsaturated groups selected from a maleimide group, a vinyl group, an allyl group, a styryl group, a vinylphenyl group, an acryloyl group, a methacryloyl group, a fumaroyl group, and a maleoyl group. Among these, from the viewpoint of providing an insulating layer with better surface smoothness, reduced smear, and well-shaped via holes, and further from the viewpoint of providing an insulating layer with little change in film thickness before and after desmearing, it is preferable that the radical polymerizable resin contains one or more selected from a maleimide resin, a (meth)acrylic resin, and a styryl resin.

[0128] The type of maleimide resin is not particularly limited as long as it has one or more (preferably two or more) maleimide groups (2,5-dihydro-2,5-dioxo-1H-pyrrol-1-yl groups) in one molecule. Examples of maleimide resins include: (1) "BMI-3000J", "BMI-5000", "BMI-1400", "BMI-1500", "BMI-1700", and "BMI-689" (all of which are available from Designer Molecules, Inc.). (1) Maleimide resins containing an aliphatic skeleton (preferably an aliphatic skeleton having 36 carbon atoms derived from dimer diamine), such as "SLK6895-T90" (manufactured by Shin-Etsu Chemical Co., Ltd.), (2) Maleimide resins containing an indane skeleton, as described in the Japan Institute of Invention and Innovation Disclosure Technical Bulletin No. 2020-500211; (3) Maleimide resins containing an aromatic ring skeleton directly bonded to the nitrogen atom of the maleimide group, such as "MIR-3000-70MT" (manufactured by Nippon Kayaku Co., Ltd.), "BMI-4000" (manufactured by Daiwa Kasei Co., Ltd.), and "BMI-80" (manufactured by Keiai Kasei Co., Ltd.).

[0129] The (meth)acrylic resin may be of any type, and may be a monomer or oligomer, as long as it has one or more (preferably two or more) (meth)acryloyl groups in one molecule. Here, the term "(meth)acryloyl group" is a general term for acryloyl groups and methacryloyl groups. Examples of methacrylic resins include (meth)acrylate monomers, as well as (meth)acrylic resins such as "A-DOG" (manufactured by Shin-Nakamura Chemical Co., Ltd.), "DCP-A" (manufactured by Kyoeisha Chemical Co., Ltd.), "NPDGA," "FM-400," "R-687," "THE-330," "PET-30," and "DPHA" (all manufactured by Nippon Kayaku Co., Ltd.).

[0130] The styryl resin is not particularly limited in type, and may be a monomer or oligomer, as long as it has one or more (preferably two or more) styryl groups or vinylphenyl groups in one molecule. Examples of the styryl resin include styrene monomers and styryl resins such as "OPE-2St," "OPE-2St 1200," and "OPE-2St 2200" (all manufactured by Mitsubishi Gas Chemical Company, Inc.).

[0131] In the multilayer resin sheet of the present invention, when the resin composition layer contains a radically polymerizable resin, the content of the radically polymerizable resin in the resin composition layer is preferably 2% by mass or more, more preferably 4% by mass or more, even more preferably 5% by mass or more, 6% by mass or more, 8% by mass or more, or 10% by mass or more, and may be increased to, for example, 12% by mass or more, 14% by mass or more, or 15% by mass or more, based on 100% by mass of the resin components in the resin composition. The upper limit of the content is not particularly limited and may be determined depending on the properties required of the resin composition, but may be, for example, 60% by mass or less, 50% by mass or less, or 40% by mass or less.

[0132] From the viewpoint of providing an insulating layer having better surface smoothness, reduced smears, and well-shaped via holes, and further from the viewpoint of providing an insulating layer with little change in film thickness before and after desmearing, it is preferred that the first resin composition layer of the resin composition layers constituting the multilayer resin sheet of the present invention contains a radical polymerizable resin.

[0133] -Curing Accelerator- In the multilayer resin sheet of the present invention, the resin composition layer may contain a curing accelerator, which allows for efficient adjustment of the curing time and curing temperature.

[0134] Examples of the curing accelerator include organic phosphine compounds such as "TPP", "TPP-K", "TPP-S", and "TPTP-S" (manufactured by Hokko Chemical Industry Co., Ltd.); imidazole compounds such as "Curesol 2MZ", "2P4MZ", "2E4MZ", "Cl1Z", "Cl1Z-CN", "Cl1Z-CNS", "Cl1Z-A", "2MZ-OK", "2MA-OK", and "2PHZ" (manufactured by Shikoku Chemical Industry Co., Ltd.); amine adduct compounds such as Novacure (manufactured by Asahi Chemical Industry Co., Ltd.) and Fujicure (manufactured by Fuji Chemical Industry Co., Ltd.); amine compounds such as 1,8-diazabicyclo[5,4,0]undecene-7,4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 4-dimethylaminopyridine; and organometallic complexes or organometallic salts of cobalt, copper, zinc, iron, nickel, manganese, tin, and the like.

[0135] When the resin composition layer in the multilayer resin sheet of the present invention contains a curing accelerator, the content of the curing accelerator in the resin composition layer is preferably 12% by mass or less, more preferably 10% by mass or less, 8% by mass or less, 6% by mass or less, or 5% by mass or less, when the resin component in the resin composition is taken as 100% by mass, from the viewpoint of easily adjusting the RD / RA ratio within a suitable range, and the lower limit may be 0.001% by mass or more, 0.01% by mass or more, 0.05% by mass or more, etc.

[0136] From the viewpoint of providing an insulating layer having better surface smoothness, reduced smears, and well-shaped via holes, and further from the viewpoint of providing an insulating layer with little change in film thickness before and after desmearing, it is preferable that the content A1 (mass%) of the curing accelerator relative to 100 mass% of the resin components in the first resin composition layer and the content A2 (mass%) of the curing accelerator relative to 100 mass% of the resin components in the layers excluding the first resin composition layer satisfy the relationship A1 > A2. The difference between A1 and A2 (A1 - A2) is preferably 1 mass% or more, more preferably 2 mass% or more, 3 mass% or more, or 4 mass% or more.

[0137] -Optional Additives- In the multilayer resin sheet of the present invention, the resin composition layer may further contain optional additives. Examples of such additives include organic fillers such as rubber particles; radical polymerization initiators such as peroxide-based radical polymerization initiators and azo-based radical polymerization initiators; organometallic compounds such as organocopper compounds, organozinc compounds, and organocobalt compounds; colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, and carbon black; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as silicone-based leveling agents and acrylic polymer-based leveling agents; thickeners such as bentone and montmorillonite; antifoaming agents such as silicone-based antifoaming agents, acrylic-based antifoaming agents, fluorine-based antifoaming agents, and vinyl resin-based antifoaming agents; ultraviolet absorbers such as benzotriazole-based ultraviolet absorbers; adhesion improvers such as urea silanes; and triazole-based adhesion-improving agents. Examples of suitable additives include adhesion promoters such as tetrazole-based adhesion promoters and triazine-based adhesion promoters; antioxidants such as hindered phenol-based antioxidants; fluorescent brightening agents such as stilbene derivatives; surfactants such as fluorine-based surfactants and silicone-based surfactants; flame retardants such as phosphorus-based flame retardants (e.g., phosphate ester compounds, phosphazene compounds, phosphinic acid compounds, and red phosphorus), nitrogen-based flame retardants (e.g., melamine sulfate), halogen-based flame retardants, and inorganic flame retardants (e.g., antimony trioxide); dispersants such as phosphate ester-based dispersants, polyoxyalkylene-based dispersants, acetylene-based dispersants, silicone-based dispersants, anionic dispersants, and cationic dispersants; and stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic anhydride-based stabilizers. The content of such additives may be determined depending on the properties required of the multilayer resin sheet.

[0138] -Method for manufacturing multilayer resin sheet- The method for manufacturing the multilayer resin sheet of the present invention is not particularly limited as long as it can realize a structure in which two or more resin composition layers are laminated on top of each other, and methods known to those skilled in the art may be used. Examples include (i) an extrusion molding method in which a resin composition is melt-kneaded using an extruder, extruded, and then molded into a film using a T-die, circular die, or the like; (ii) a casting molding method in which a resin composition is dissolved or dispersed in a solvent, and then cast to form a film; and (iii) other conventionally known film molding methods. Among these, the extrusion molding method and the casting molding method are preferred because they can be used to achieve thinner sheets. The multilayer resin sheet of the present invention includes two or more resin composition layers laminated on top of each other. Examples of methods for forming a multilayer resin sheet by laminating two or more resin composition layers on top of each other include (1) a method for forming a multilayer resin sheet by simultaneously or sequentially forming resin composition layers during coating or extrusion, (2) a method for forming a multilayer resin sheet by laminating two or more resin composition layers that have been prepared separately using a heat roll laminator or the like, (3) a method for forming a resin sheet having a multilayer structure in a single resin sheet by causing differences in the contents of each component in the resin sheet during casting molding, and (4) other conventionally known methods for forming a multilayer resin sheet.

[0139] A preferred example of a method for producing a multilayer resin sheet having two resin composition layers, i.e., a first resin composition layer and a second resin composition layer, will be described below.

[0140] In one embodiment, a method for producing a multilayer resin sheet includes: (A1) a step of preparing a supported resin sheet including a support and a first resin composition layer bonded to the support; and (B1) a step of applying a second resin composition onto the first resin composition layer and drying the applied film to provide the second resin composition layer (hereinafter, such an embodiment of lamination by coating will also be referred to as a "first embodiment").

[0141] In step (A1), a resin sheet with a support is prepared, the resin sheet including a support and a first resin composition layer bonded to the support. The support will be described later in the section "Support-Attached Multilayer Resin Sheet."

[0142] The resin sheet with a support can be produced, for example, by applying the first resin composition to a support and drying the coating film to provide a first resin composition layer. Specifically, the resin sheet can be produced by dissolving the first resin composition in an organic solvent to prepare a resin varnish, applying the resin varnish to a support using a die coater or the like, and drying the coating film.

[0143] Examples of organic solvents include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; ether-based solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, and diphenyl ether; alcohol-based solvents such as methanol, ethanol, propanol, butanol, and ethylene glycol; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, and methyl methoxypropionate. ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, diethylene glycol monobutyl ether (butyl carbitol), and the like; amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone; sulfoxide solvents such as dimethyl sulfoxide; nitrile solvents such as acetonitrile and propionitrile; aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane; and aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. The organic solvent may be used alone or in combination of two or more.

[0144] The coating film may be dried by a known drying method such as heating, blowing hot air, etc. Although the drying method varies depending on the boiling point of the organic solvent in the resin varnish, for example, when a resin varnish containing 30% by mass to 60% by mass of an organic solvent is used, the first resin composition layer can be formed on the support by drying at 80° C. to 180° C. for 2 minutes to 10 minutes.

[0145] In step (B1), a second resin composition is applied onto the first resin composition layer, and the applied film is dried to provide a second resin composition layer, thereby forming a supported multilayer resin sheet in which a multilayer resin sheet is formed on the support.

[0146] The application of the second resin composition and the drying of the coating film may be carried out in the same manner as the application of the first resin composition and the drying of the coating film in step (A1). From the viewpoint of easily adjusting the RD / RA ratio within a suitable range, when the drying temperature (°C) of the coating film in step (A1) is T1 and the drying temperature (°C) of the coating film in step (A2) is T2, it is preferable to satisfy the relationship of preferably T1>T2, more preferably T1≧(T2+20), and even more preferably T1≧(T2+40) or T1≧(T2+50).

[0147] The multilayer resin sheet with a support may further include a protective film equivalent to the support on the surface of the multilayer resin sheet that is not bonded to the support (i.e., the surface opposite to the support). When a protective film is provided, the multilayer resin sheet with a support can be used by peeling off the protective film when laminating it on a target member to be laminated.

[0148] In another embodiment, the method for producing a multilayer resin sheet includes: (A2a) a step of preparing a first supported resin sheet including a first support and a first resin composition layer bonded to the first support; (A2b) a step of preparing a second supported resin sheet including a second support and a second resin composition layer bonded to the second support; and (B2) a step of laminating the first supported resin sheet and the second supported resin sheet together so that the first resin composition layer and the second resin composition layer are bonded to each other (hereinafter, this embodiment of lamination by lamination will also be referred to as a "second embodiment").

[0149] In the second embodiment, step (A2a) and step (A2b) may each be performed in the same manner as step (A1) in the first embodiment. Here, from the viewpoint of easily adjusting the RD / RA ratio within a suitable range, when the drying temperature (°C) of the coating film in step (A2a) is Ta and the drying temperature (°C) of the coating film in step (A2b) is Tb, it is preferable that the relationship of Ta > Tb, more preferably Ta ≥ (Tb + 20), and even more preferably Ta ≥ (Tb + 40) or Ta ≥ (Tb + 50) is satisfied.

[0150] In step (B2), the first supported resin sheet and the second supported resin sheet are laminated so that the first resin composition layer and the second resin composition layer are bonded. This forms a multilayer resin sheet between the first support and the second support. The second support can function as the protective film in the first embodiment. The supported multilayer resin sheet produced in the second embodiment can be used by peeling off the second support (protective film) when laminating it to a member to be laminated.

[0151] For the lamination in step (B2), the lamination temperature is preferably in the range of 60°C to 160°C, more preferably 80°C to 140°C, the lamination pressure is preferably in the range of 0.098 MPa to 1.77 MPa, more preferably 0.29 MPa to 1.47 MPa, and the lamination time is preferably in the range of 20 seconds to 400 seconds, more preferably 30 seconds to 300 seconds. Lamination can be carried out under reduced pressure conditions, preferably a pressure of 26.7 hPa or less.

[0152] Lamination can be performed using a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch-type vacuum pressure laminator.

[0153] The multilayer resin sheet of the present invention can provide an insulating layer with good surface smoothness, reduced smearing, and well-shaped via holes, even when a desmear treatment is performed after peeling off the support. The multilayer resin sheet of the present invention can also provide an insulating layer with little change in film thickness before and after the desmear treatment. Therefore, the multilayer resin sheet of the present invention can be suitably used as a multilayer resin sheet for forming an insulating layer of a printed wiring board (a multilayer resin sheet for an insulating layer of a printed wiring board), and more suitably used as a multilayer resin sheet for forming an interlayer insulating layer of a printed wiring board (a multilayer resin sheet for an interlayer insulating layer of a printed wiring board). The multilayer resin sheet of the present invention can also be suitably used when the printed wiring board is a circuit board with built-in components. The resin composition of the present invention can also be suitably used as a multilayer resin sheet for forming an insulating layer (a multilayer resin sheet for an insulating layer for forming a conductor layer) in contact with the insulating layer on which a conductor layer (including a rewiring layer) will be formed.

[0154] [Support-Attached Multilayer Resin Sheet] The present invention also provides a supported multilayer resin sheet in which the multilayer resin sheet of the present invention is provided on a support.

[0155] The multilayer resin sheet with a support of the present invention comprises the multilayer resin sheet of the present invention and a support bonded to the first resin composition layer of the multilayer resin sheet.

[0156] The multilayer resin sheet of the present invention is as described above in the section [Multilayer Resin Sheet]. In the supported multilayer resin sheet of the present invention, the first resin composition layer of the multilayer resin sheet of the present invention is bonded to the support.

[0157] Examples of the support include a thermoplastic resin film, a metal foil, and a release paper, and a thermoplastic resin film or a metal foil is preferred. Therefore, in a preferred embodiment, the support is a thermoplastic resin film or a metal foil.

[0158] When a thermoplastic resin film is used as the support, examples of the thermoplastic resin include polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), acrylics such as polycarbonate (PC) and polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0159] When a metal foil is used as the support, examples of the metal foil include copper foil and aluminum foil, with copper foil being preferred. The copper foil may be a foil made of a single metal, such as copper, or a foil made of an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.).

[0160] The support may be subjected to a matte treatment, a corona treatment, or an antistatic treatment on the surface that will be bonded to the first resin composition layer. Alternatively, a support with a release layer, which has a release layer on the surface that will be bonded to the first resin composition layer, may be used as the support. Examples of the release agent used in the release layer of the support with a release layer include one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. Commercially available products may be used as the support with a release layer, including, for example, "SK-1," "AL-5," and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Uni-Peel" manufactured by Unitika Ltd., which are PET films having a release layer primarily composed of an alkyd resin-based release agent.

[0161] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the thickness of the entire support with a release layer is in the above range.

[0162] In one embodiment, the multilayer resin sheet with a support may further include an optional layer, if necessary. Examples of such optional layers include a protective film provided on the surface of the multilayer resin sheet that is not bonded to the support (i.e., the surface opposite the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating a protective film, it is possible to prevent the adhesion of dust and the like to the surface of the multilayer resin sheet and to prevent scratches.

[0163] The method for producing the multilayer resin sheet with a support is as explained above in the section "Multilayer resin sheet."

[0164] The multilayer resin sheet with a support can be wound up into a roll and stored. When the resin sheet with a support has a protective film, it can be used by peeling off the protective film. Here, when the adhesive strength between the support and the multilayer resin sheet (specifically, the first resin composition layer) is S1 and the adhesive strength between the protective film and the multilayer resin sheet (specifically, the outermost layer opposite the first resin composition layer) is S2, the relationship S1 > S2 is satisfied. This allows the protective film to be peeled off from the multilayer resin sheet before the support, exposing the surface of the multilayer resin sheet opposite the first resin composition layer, and ultimately allowing the multilayer resin sheet to be laminated so that the surface of the multilayer resin sheet opposite the first resin composition layer is bonded to a target member.

[0165] The supported multilayer resin sheet of the present invention can be suitably used for forming an insulating layer of a printed wiring board (for an insulating layer of a printed wiring board), and can be more suitably used for forming an interlayer insulating layer of a printed wiring board (for an interlayer insulating layer of a printed wiring board). The sheet-like laminate material of the present invention can also be suitably used as a resin composition for forming an insulating layer (for an insulating layer for forming a conductor layer) on which a conductor layer (including a rewiring layer) will be formed in contact therewith.

[0166] [Printed Wiring Board] The printed wiring board of the present invention includes an insulating layer made of a cured product of the multilayer resin sheet of the present invention.

[0167] A printed wiring board can be produced, for example, by a method including the following steps (I) to (IV) using the multilayer resin sheet of the present invention: (I) a step of laminating the multilayer resin sheet of the present invention on an inner layer substrate so that the surface of the multilayer resin sheet opposite to the first resin composition layer is bonded to the inner layer substrate, (II) a step of curing (e.g., thermally curing) the multilayer resin sheet to form an insulating layer, (III) a step of forming via holes in the insulating layer with a laser and performing a desmear treatment, and (IV) a step of forming a metal film on the surface of the insulating layer after the desmear treatment.

[0168] -Step (I)- In step (I), the multilayer resin sheet of the present invention is laminated on an inner layer substrate so that the surface of the multilayer resin sheet opposite the first resin composition layer is bonded to the inner layer substrate.

[0169] The "inner layer substrate" used in step (I) is a member that will become the substrate of a printed wiring board, and examples thereof include glass epoxy substrates, metal substrates, polyester substrates, polyimide substrates, BT resin substrates, and thermosetting polyphenylene ether substrates. The substrate may have a conductor layer on one or both sides, and this conductor layer may be patterned. An inner layer substrate having a conductor layer (circuit) formed on one or both sides of the substrate is sometimes referred to as an "inner layer circuit board." Furthermore, intermediate products on which an insulating layer and / or a conductor layer is to be further formed during the production of a printed wiring board are also included in the "inner layer substrate" of the present invention. When the printed wiring board is a circuit board with built-in components, an inner layer substrate with built-in components may be used.

[0170] The lamination of the inner layer substrate and the multilayer resin sheet can be carried out, for example, by using the multilayer resin sheet with a support of the present invention and thermocompressing the multilayer resin sheet to the inner layer substrate from the support side. Examples of a member for thermocompressing the multilayer resin sheet to the inner layer substrate (hereinafter also referred to as a "thermocompression member") include a heated metal plate (such as a SUS panel) or a metal roll (such as a SUS roll). The thermocompression member may be pressed directly onto the multilayer resin sheet with a support, or may be pressed via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently conform to the surface irregularities of the inner layer substrate.

[0171] The lamination of the inner layer substrate and the multilayer resin sheet may be carried out by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098 MPa to 1.77 MPa, more preferably 0.29 MPa to 1.47 MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably 30 seconds to 300 seconds. The lamination may be carried out under reduced pressure conditions, preferably a pressure of 26.7 hPa or less.

[0172] The lamination can be performed using a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch-type vacuum pressure laminator.

[0173] After lamination, the laminated multilayer resin sheet may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for lamination. The smoothing treatment may be performed using a commercially available laminator. Note that lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.

[0174] The support may be removed between step (I) and step (II), or may be removed after step (II). When a metal foil is used as the support, the conductor layer may be formed using the metal foil without peeling off the support.

[0175] -Step (II)- In step (II), the multilayer resin sheet is cured (for example, thermally cured) to form an insulating layer made of the cured product of the multilayer resin sheet.

[0176] The conditions for curing the multilayer resin sheet are not particularly limited, and conditions that are usually employed when forming an insulating layer for a printed wiring board may be used.

[0177] For example, the heat curing conditions for the multilayer resin sheet vary depending on the composition of the resin composition layer, etc., but in one embodiment, the curing temperature is preferably 120° C. to 250° C., more preferably 150° C. to 240° C., and even more preferably 170° C. to 230° C. The curing time is preferably 5 minutes to 240 minutes, more preferably 10 minutes to 150 minutes, and even more preferably 15 minutes to 120 minutes.

[0178] Before thermally curing the multilayer resin sheet, the multilayer resin sheet may be preheated at a temperature lower than the curing temperature. For example, prior to thermally curing the multilayer resin sheet, the multilayer resin sheet may be preheated at a temperature of 50°C to 120°C, preferably 60°C to 115°C, more preferably 70°C to 110°C for 5 minutes or more, preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and even more preferably 15 minutes to 100 minutes.

[0179] -Step (III)- In step (III), via holes are formed in the insulating layer with a laser, and a desmear treatment is performed.

[0180] The laser light source for forming the via holes in the insulating layer is, for example, a carbon dioxide laser (CO 2 Laser), UV-YAG laser, excimer laser, etc. may be used as the light source. Among them, from the viewpoint of being able to enjoy the effects of the present invention more effectively, CO 2 Preferably, a laser is used. Thus, in one embodiment, the insulating layer is 2 A via hole is formed using a laser.

[0181] The dimensions and shape of the via hole may be appropriately determined depending on the design of the printed wiring board. For example, the shape of the via hole is not particularly limited, but is generally circular (approximately circular). The top diameter of the via hole is preferably 50 μm or less, 40 μm or less, 30 μm or less, or 20 μm or less, and the lower limit may be, for example, 3 μm or more, 5 μm or more, 10 μm or more, etc. Here, the top diameter of the via hole refers to the diameter of the opening of the via hole at the insulating layer surface (the insulating layer surface derived from the first resin composition layer).

[0182] By using the multilayer resin sheet of the present invention, it is possible to form via holes with a good cross-sectional shape that exhibits minimal dimensional change in the thickness direction of the insulating layer. In one embodiment, when observing the cross section of the via hole, the relationship R1 ≧ R2 is satisfied, where R1 is the maximum via diameter (μm) in the insulating layer portion derived from the first resin composition layer and R2 is the maximum via diameter (μm) in the insulating layer portion derived from layers other than the first resin composition layer. In a preferred embodiment, R1 and R2 satisfy the relationship R1 ≧ R2 and also satisfy the relationship (R1 − R2) ≦ 0.1R1.

[0183] After forming via holes in an insulating layer with a laser, a desmear treatment is performed. This allows resin residue (smear) in the via holes to be removed. The procedure and conditions for the desmear treatment are not particularly limited, and known procedures and conditions that are commonly used when forming insulating layers for printed wiring boards can be adopted. For example, the desmear treatment can be performed by carrying out a swelling treatment using a swelling liquid, a desmear (roughening) treatment using an oxidizing agent liquid, and a neutralization treatment using a neutralizing liquid in this order.

[0184] The swelling liquid used in the desmear treatment is not particularly limited, but examples thereof include alkaline solutions and surfactant solutions, and is preferably an alkaline solution, with sodium hydroxide solution and potassium hydroxide solution being more preferred. Commercially available swelling liquids include "Swelling Dip Securigant P" and "Swelling Dip Securigant SBU" manufactured by Atotech Japan. The swelling treatment using a swelling liquid is not particularly limited, but can be carried out by, for example, immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 to 20 minutes. From the viewpoint of suppressing swelling of the resin in the insulating layer to an appropriate level, it is preferable to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 to 15 minutes.

[0185] The oxidizing agent solution used in the desmear treatment is not particularly limited, but examples thereof include alkaline permanganate solutions prepared by dissolving potassium permanganate or sodium permanganate in an aqueous solution of sodium hydroxide. Roughening treatment using an oxidizing agent solution such as an alkaline permanganate solution is preferably carried out by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 100°C for 10 minutes to 30 minutes. The concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securigans P" manufactured by Atotech Japan.

[0186] The neutralizing solution used in the desmear treatment is preferably an acidic aqueous solution, and a commercially available product such as "Reduction Securiganth P" manufactured by Atotech Japan Ltd. Neutralization treatment with a neutralizing solution can be carried out by immersing the surface that has been roughened with an oxidizing agent in the neutralizing solution at 30°C to 80°C for 5 to 30 minutes. From the standpoint of workability and the like, a method in which the object that has been roughened with an oxidizing agent is immersed in the neutralizing solution at 40°C to 70°C for 5 to 20 minutes is preferred.

[0187] Here, when the desmear treatment is carried out after peeling off the support, the desmear treatment also serves as a roughening treatment for the exposed surface of the insulating layer. As described above, the multilayer resin sheet of the present invention is advantageous because it can provide an insulating layer with good surface smoothness, reduced smears, and well-shaped via holes, even when the desmear treatment is carried out after peeling off the support. Therefore, in one embodiment, the desmear treatment is carried out after peeling off the support. In a preferred embodiment, step (III) is a step of forming via holes in the insulating layer with a laser, peeling off the support, and then carrying out the desmear treatment.

[0188] -Step (IV)- After the desmear treatment in step (III), a metal film is formed on the surface of the insulating layer in step (IV). The formed metal film can be used as a plating seed layer to form wiring.

[0189] The thickness of the metal film (plating seed layer) may be preferably 500 nm or less, more preferably 400 nm or less, and even more preferably 300 nm or less. After a conductor layer is formed on the metal film in a desired pattern, unnecessary portions other than the conductor layer formation portion are removed by etching or the like. In this case, the thinner the metal film, the easier it is to remove the unnecessary portions of the metal film, and the smaller the thickness of the metal film, the more easily erosion of the conductor pattern can be minimized when removing the unnecessary portions, which is advantageous for realizing fine wiring.

[0190] In this regard, when a thin metal film is formed on the surface of an insulating layer, the thickness of the conductor layer formed on the metal film by electroplating tends to vary, resulting in a phenomenon known as plating burn. This is thought to be due to the unevenness of the metal film caused by the unevenness of the insulating layer surface. Specifically, the electrical resistance of the thin metal film is higher than that of the thick metal film. When a conductor layer is formed on the thin metal film by electroplating, the plating growth is delayed in the thin metal film and high electrical resistance areas compared to other areas, resulting in insufficient formation of the conductor layer and making it difficult to form a uniform conductor layer.

[0191] In contrast, by using the multilayer resin sheet of the present invention, an insulating layer with excellent surface smoothness can be formed, and plating burn can be suppressed even if the thickness of the metal film is made thinner, for example, the thickness of the metal film may be reduced to 280 nm or less, 260 nm or less, or 250 nm or less.

[0192] The metal film (plating seed layer) includes at least a conductive seed layer. The conductive seed layer functions as an electrode in an electrolytic plating method. The conductive material constituting the conductive seed layer is not particularly limited as long as it exhibits sufficient conductivity, and suitable examples include copper, palladium, gold, platinum, silver, aluminum, and alloys thereof. The metal film may also include a diffusion barrier layer. The diffusion barrier layer is a layer that prevents the conductive material constituting the conductive seed layer from diffusing into the insulating layer and causing dielectric breakdown. The material constituting the diffusion barrier layer is also not particularly limited as long as it can suppress or prevent the diffusion of the conductive material constituting the conductive seed layer, and suitable examples include titanium, tungsten, tantalum, and alloys thereof. When the metal film includes a diffusion barrier layer, the "thickness of the metal film" in the present invention refers to the average thickness of the entire metal film, including not only the conductive seed layer but also the diffusion barrier layer.

[0193] When the metal film includes a diffusion barrier layer, the thickness of the diffusion barrier layer is not particularly limited as long as it can suppress or prevent the diffusion of the conductive material constituting the conductive seed layer, but from the viewpoint of contributing to the realization of fine wiring, it is preferably 50 nm or less, more preferably 40 nm or less, and even more preferably 30 nm or less. The lower limit of the thickness of the diffusion barrier layer is not particularly limited and may be, for example, 1 nm or more, 3 nm or more, 5 nm or more, etc. In this case, the remainder of the metal film is preferably a conductive seed layer, and the thickness of the conductive seed layer may be determined in relation to the thickness of the diffusion barrier layer so that the thickness of the entire metal film falls within the above-mentioned preferred range.

[0194] The metal film may be formed by dry plating or wet plating. Examples of dry plating include physical vapor deposition (PVD) methods such as sputtering, ion plating, and vacuum deposition, and chemical vapor deposition (CVD) methods such as thermal CVD and plasma CVD. Examples of wet plating include electroless plating. Sputtering and electroless plating are preferred from the viewpoint of easily forming a thin metal film with a more uniform thickness, and sputtering is particularly preferred from the viewpoint of realizing fine wiring with excellent adhesion strength. Therefore, in a preferred embodiment, the metal film is formed by sputtering in step (IV).

[0195] After step (IV), a conductor layer can be formed on the metal film by electroplating. Thus, in one embodiment, the method for producing a printed wiring board of the present invention includes, as step (V), a step of forming a conductor layer on the metal film by electroplating.

[0196] The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin, and indium. The conductor layer may be a single metal layer or an alloy layer. Examples of the alloy layer include a layer formed from an alloy of two or more metals selected from the above group (e.g., a nickel-chromium alloy, a copper-nickel alloy, and a copper-titanium alloy). Among these, from the viewpoints of versatility, cost, ease of patterning, etc., in forming the conductor layer, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy, or a copper-titanium alloy is preferred. A single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.

[0197] The conductor layer may have a single layer structure or a multi-layer structure in which two or more single metal layers or alloy layers made of different types of metals or alloys are stacked. When the conductor layer has a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc, or titanium, or an alloy layer of a nickel-chromium alloy.

[0198] The thickness of the conductor layer depends on the desired design of the printed wiring board, but is generally 3 μm to 35 μm, preferably 5 μm to 30 μm.

[0199] The formation of the conductor layer may be carried out by a so-called semi-additive method. That is, a photoresist (plating resist) is formed on the metal film formed in step (IV), exposing a portion of the metal film corresponding to the desired wiring pattern. Next, a conductor layer is formed on the exposed metal film by electrolytic plating, and the photoresist is then removed. Thereafter, unnecessary metal film other than the conductor layer formation portion is removed by etching or the like, thereby forming a conductor layer (wiring) having the desired wiring pattern.

[0200] By using the multilayer resin sheet of the present invention, it is possible to form a fine conductor circuit with an L / S of, for example, 5 / 5 μm or less, 4 / 4 μm or less, 3 / 3 μm or less, 2 / 2 μm or less, 1.5 / 1.5 μm or less, or 1 / 1 μm or less while suppressing plating burn.

[0201] If necessary, the steps (I) to (V) for forming the insulating layer and the conductor layer may be repeated to form a multilayer wiring board.

[0202] [Semiconductor Chip Package] A semiconductor chip package can be produced using the multilayer resin sheet of the present invention. The present invention also provides such a semiconductor chip package. The semiconductor chip package of the present invention includes an insulating layer (rewiring formation layer) for forming a rewiring layer, which is made of a cured product of the multilayer resin sheet of the present invention.

[0203] A semiconductor chip package can be manufactured, for example, by a method including the following steps (1) to (6) using the multilayer resin sheet of the present invention. The multilayer resin sheet of the present invention can be used to form the rewiring formation layer in step (5). An example of forming a rewiring formation layer using a multilayer resin sheet is shown below. However, techniques for forming a rewiring formation layer for a semiconductor chip package are known, and a person skilled in the art can manufacture a semiconductor package using the multilayer resin sheet of the present invention according to known techniques. (1) A step of laminating a temporary fixing film on a substrate; (2) A step of temporarily fixing a semiconductor chip on the temporary fixing film; (3) A step of forming a sealing layer on the semiconductor chip; (4) A step of peeling the substrate and the temporary fixing film from the semiconductor chip; (5) A step of forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the substrate and the temporary fixing film have been peeled; and (6) A step of forming a rewiring layer as a conductor layer on the rewiring formation layer.

[0204] -Step (1)- The material used for the substrate is not particularly limited. Examples of the substrate include a silicon wafer, a glass wafer, a glass substrate, a metal substrate such as copper, titanium, stainless steel, or cold-rolled steel plate (SPCC), a substrate in which glass fiber is impregnated with an epoxy resin or the like and subjected to a thermosetting treatment (e.g., an FR-4 substrate), and a substrate made of bismaleimide triazine resin (BT resin).

[0205] The material of the temporary fixing film is not particularly limited as long as it can be peeled off from the semiconductor chip in step (4) and can temporarily fix the semiconductor chip. Commercially available products can be used as the temporary fixing film. Examples of commercially available products include Riva Alpha manufactured by Nitto Denko Corporation.

[0206] -Step (2)- The semiconductor chips can be temporarily fixed using known devices such as a flip chip bonder, a die bonder, etc. The layout and number of semiconductor chips to be arranged can be set appropriately depending on the shape and size of the temporary fixing film, the number of semiconductor packages to be produced, etc. For example, the semiconductor chips can be temporarily fixed by arranging them in a matrix of multiple rows and multiple columns.

[0207] -Step (3)- An encapsulating resin sheet having an encapsulating resin composition layer provided on a support is laminated on a semiconductor chip, or an encapsulating resin composition is applied on a semiconductor chip and cured (for example, thermally cured) to form an encapsulating layer.

[0208] For example, the semiconductor chip and the sealing resin sheet can be laminated by thermocompression bonding the sealing resin sheet to the semiconductor chip from the support side. The semiconductor chip and the sealing resin sheet may be laminated by a vacuum lamination method, and the lamination conditions are the same as those described in relation to the method for producing a printed wiring board, and the preferred ranges are also the same.

[0209] After lamination, the encapsulating resin composition layer is thermally cured to form an encapsulating layer, under the same conditions as those described in relation to the method for producing a printed wiring board.

[0210] The support of the sealing resin sheet may be peeled off after the sealing resin sheet is laminated on the semiconductor chip and thermally cured, or the support may be peeled off before the sealing resin sheet is laminated on the semiconductor chip.

[0211] When the encapsulating layer is formed by applying the encapsulating resin composition, the application conditions are the same as the application conditions for forming the resin composition layer described in relation to the method for producing the multilayer resin sheet of the present invention, and the preferred ranges are also the same.

[0212] -Step (4)- The method for peeling off the substrate and the temporary fixing film can be changed as appropriate depending on the material of the temporary fixing film, etc., and examples thereof include a method in which the temporary fixing film is heated and foamed (or expanded) to peel off, and a method in which ultraviolet light is irradiated from the substrate side to reduce the adhesive strength of the temporary fixing film and then peel it off.

[0213] In the method of heating and foaming (or expanding) the temporary fixing film to peel it off, the heating conditions are usually 100 to 250°C for 1 to 90 seconds or 5 to 15 minutes. In the method of irradiating ultraviolet light from the substrate side to reduce the adhesive strength of the temporary fixing film to peel it off, the irradiation dose of ultraviolet light is usually 10 mJ / cm. 2 ~1000mJ / cm 2 is.

[0214] Step (5) - The material for forming the rewiring formation layer (insulating layer) is not particularly limited as long as it has insulating properties when the rewiring formation layer (insulating layer) is formed, and the rewiring formation layer can be formed using the multilayer resin sheet of the present invention. In step (5), the multilayer resin sheet of the present invention is laminated so that the surface opposite to the first resin composition layer is bonded to the surface of the semiconductor chip from which the substrate and the temporary fixing film have been peeled. Thereafter, the multilayer resin sheet is cured to form the rewiring formation layer.

[0215] After forming the redistribution layer, via holes may be formed in the redistribution layer to connect the semiconductor chip to a conductor layer (described later). The via holes may be formed by a known method depending on the material of the redistribution layer.

[0216] Step (6)—The formation of a conductor layer on the rewiring formation layer may be carried out in the same manner as step (V) described in relation to the method for producing a printed wiring board. Steps (5) and (6) may be repeated to alternately stack (build up) conductor layers (rewiring layers) and rewiring formation layers (insulating layers).

[0217] The manufacturing of the semiconductor chip package may further include steps of (7) forming a solder resist layer on the conductor layer (rewiring layer), (8) forming bumps, and (9) dicing the plurality of semiconductor chip packages into individual semiconductor chip packages. These steps may be performed according to various methods known to those skilled in the art for use in manufacturing semiconductor chip packages.

[0218] By forming a rewiring formation layer using the multilayer resin sheet of the present invention, a semiconductor chip package can be realized regardless of whether the semiconductor package is a fan-in package or a fan-out package. Furthermore, the multilayer resin sheet of the present invention can be applied to both a fan-out panel level package (FO-PLP) and a fan-out wafer level package (FO-WLP).

[0219] [Semiconductor Device] The semiconductor device of the present invention includes a layer made of a cured product of the multilayer resin sheet of the present invention. The semiconductor device of the present invention can be produced using the printed wiring board or semiconductor chip package of the present invention.

[0220] Examples of semiconductor devices include various semiconductor devices used in electrical appliances (for example, computers, mobile phones, digital cameras, and televisions) and vehicles (for example, motorcycles, automobiles, trains, ships, and aircraft).

[0221] The present invention will be specifically described below by way of examples and comparative examples, but the present invention is not limited to the following examples.

[0222] (Thermosetting Resin) (1) Biphenyl type epoxy resin ("NC-3000" manufactured by Nippon Kayaku Co., Ltd.) (2) Biphenyl type epoxy resin ("NC-3000-H" manufactured by Nippon Kayaku Co., Ltd.) (3) p-Aminophenol type epoxy resin ("630" manufactured by Mitsubishi Chemical Corporation) (4) Dicyclopentadiene type epoxy resin ("HP-7200" manufactured by DIC Corporation)

[0223] (Curing Agent) (1) Aminotriazine skeleton cresol novolac resin-containing liquid (DIC Corporation's "LA-3018-50P", containing 50% by mass of non-volatile components and 50% by mass of propylene glycol monoethyl ether) (2) Triazine skeleton phenol novolac resin-containing liquid (DIC Corporation's "LA-7054", containing 60% by mass of non-volatile components and 40% by mass of methyl ethyl ketone) (3) Active ester resin-containing liquid (DIC Corporation's "HPC-8000-65T", containing 65% by mass of non-volatile components and 35% by mass of toluene)

[0224] (Curing Accelerator) (1) Imidazole Compound (2-phenyl-4-methylimidazole, "2P4MZ" manufactured by Shikoku Chemicals Corporation)

[0225] (Thermoplastic Resins) (1) Phenoxy resin-containing liquid ("YX6954BH30" manufactured by Mitsubishi Chemical Corporation, containing 30% by mass of non-volatile components, 35% by mass of methyl ethyl ketone, and 35% by mass of cyclohexanone) (2) Polyimide resin 1 (polyimide resin synthesized in Synthesis Example 1 below, containing 20% ​​by mass of non-volatile components)

[0226] (Radical Polymerizable Resin) Maleimide Resin 1 (SLK6895-T90, an aliphatic skeleton-containing maleimide resin having a structure represented by the following formula (which may partially contain unsaturated bonds), 90% by mass of non-volatile components and 10% by mass of toluene)

[0227]

[0228] (Inorganic fillers) (1) Silica 1 (spherical silica obtained by surface-treating 100 parts by mass of "SO-C4" manufactured by Admatechs with 0.4 parts by mass of a silane coupling agent having an N-phenyl-3-aminopropyl group ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.), average particle size: 1.0 μm) (2) Silica 2 (spherical silica obtained by surface-treating 100 parts by mass of "SO-C2" manufactured by Admatechs with 0.6 parts by mass of a silane coupling agent having an N-phenyl-3-aminopropyl group ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.), average particle size: 0.5 μm) (3) Silica 3 (spherical silica obtained by surface-treating 100 parts by mass of "YC100C" manufactured by Admatechs with 3.0 parts by mass of a silane coupling agent having an N-phenyl-3-aminopropyl group ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.), average particle size: 0.10 μm)

[0229] (Solvent) (1) Solvent (MEK, methyl ethyl ketone, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)

[0230] Synthesis Example 1: Polyimide Resin 1 A monomer composition was prepared by mixing 49.6 g of 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (hereinafter also referred to as "BPADA"), 50.4 g of 4,4'-[1,4-phenylenebis[(1-methylethylidene)-4,1-phenyleneoxy]]bisbenzenamine (hereinafter also referred to as "BPPAN"), and 40 g of toluene as a solvent into 400 g of N,N-dimethylacetamide (hereinafter also referred to as "DMAc") as a solvent. The resulting mixture was stirred and reacted at room temperature and atmospheric pressure for 3 hours. This produced a polyamic acid solution.

[0231] Subsequently, the polyamic acid solution was heated and maintained at approximately 160°C, and the condensed water was azeotropically removed with toluene under a nitrogen stream. It was confirmed that a predetermined amount of water had accumulated in the water content receiver and that no water was leaking out. After confirmation, the reaction solution was further heated and stirred at 200°C for 1 hour. It was then cooled. This yielded a varnish containing 20% ​​by mass of polyimide resin (hereinafter also referred to as "polyimide resin 1") as a non-volatile component.

[0232] From the above reaction pathway, it was estimated that polyimide resin 1 contained a structural unit represented by the following formula (C1a): Furthermore, from the above reaction pathway, it was estimated that polyimide resin 1 contained a first skeleton derived from BPADA and a second skeleton derived from BPPAN.

[0233]

[0234] The glass transition temperature Tg (TMA method) of Polyimide Resin 1 was 210° C. Tg was measured using a TMA device manufactured by Rigaku Corporation at a temperature rise rate of 5° C. / min from 25° C. to 250° C.

[0235] Example 1 A mixture of 25 parts by mass of biphenyl-type epoxy resin (manufactured by Nippon Kayaku Co., Ltd., "NC-3000"), 2 parts by mass of bisphenol-type epoxy resin (manufactured by Nippon Steel Chemical & Material Co., Ltd., "ZX1059"), 7 parts by mass of dicyclopentadiene-type epoxy resin (manufactured by DIC Corporation, "HP-7200"), 5 parts by mass (non-volatile components: 2.5 parts by mass) of an aminotriazine-skeleton cresol novolac resin-containing liquid (manufactured by DIC Corporation, "LA-3018-50P"), and an active ester resin-containing liquid (manufactured by DIC Corporation, "HPC-8000-65T") was used. 200 parts by mass of a polyimide resin (130 parts by mass of non-volatile components), 10 parts by mass of an imidazole compound ("2P4MZ" manufactured by Shikoku Chemical Industry Co., Ltd.), 10 parts by mass of a phenoxy resin-containing liquid ("YX6954BH30" manufactured by Mitsubishi Chemical Corporation) (3 parts by mass of non-volatile components), 15 parts by mass of a maleimide resin (13.5 parts by mass of non-volatile components), 5 parts by mass of a polyimide resin 1 (1 part by mass of non-volatile components), and 125 parts by mass of methyl ethyl ketone (MEK) were mixed and stirred at room temperature until a uniform solution was obtained, thereby obtaining a resin composition varnish A.

[0236] Formation of outer layer (first resin composition layer; layer that becomes the outer layer after lamination): The obtained resin composition varnish A was mixed with 130 parts by mass of silica 3 (spherical silica obtained by surface-treating 100 parts by mass of "YC100C" manufactured by Admatechs with 3.0 parts by mass of a silane coupling agent having an N-phenyl-3-aminopropyl group ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.), and the mixture was stirred at room temperature until a uniform solution was obtained, thereby obtaining a resin composition varnish B.

[0237] The obtained resin composition varnish B was applied to the release-treated surface of a PET film (thickness: 38 μm) using an applicator, and then dried for 180 seconds in a gear oven at 170° C. to volatilize the solvent. In this way, a sheet-like molded product A (outer layer: first resin composition layer) having a thickness of 2 μm was obtained on the PET film.

[0238] Formation of inner layer (layers other than the first resin composition layer; layers that will become inner layers after lamination): Formation method 1 - Lamination by coating 20 parts by mass of biphenyl type epoxy resin ("NC-3000" manufactured by Nippon Kayaku Co., Ltd.), 3 parts by mass of bisphenol type epoxy resin ("ZX1059" manufactured by Nippon Steel Chemical & Material Co., Ltd.), 10 parts by mass of dicyclopentadiene type epoxy resin ("HP-7200" manufactured by DIC Corporation), 15 parts by mass (7.5 parts by mass of non-volatile components) of aminotriazine skeleton cresol novolac resin-containing liquid ("LA-3018-50P" manufactured by DIC Corporation), and active ester resin-containing liquid ("DIC Corporation"). A resin composition varnish C was obtained by mixing 80 parts by mass (52 parts non-volatile components) of a polyimide resin ("HPC-8000-65T" manufactured by Shikoku Chemicals Corporation), 2 parts by mass of an imidazole compound ("2P4MZ" manufactured by Shikoku Chemicals Corporation), 5 parts by mass (1.5 parts by mass of non-volatile components) of a phenoxy resin-containing liquid ("YX6954BH30" manufactured by Mitsubishi Chemical Corporation), 5 parts by mass of polyimide resin 1 (1 part by mass of non-volatile components), and 200 parts by mass of methyl ethyl ketone (MEK), and stirring at room temperature until a homogeneous solution was obtained.

[0239] The obtained resin composition varnish C was mixed with 290 parts by mass of silica 2 (spherical silica obtained by surface-treating 100 parts by mass of "SO-C2" manufactured by Admatechs Co., Ltd. with 0.6 parts by mass of a silane coupling agent having an N-phenyl-3-aminopropyl group ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.), and the mixture was stirred at room temperature until a uniform solution was obtained, thereby obtaining resin composition varnish D.

[0240] Next, the obtained resin composition varnish D was applied to the obtained sheet-like molded body A so that the total thickness was 40 μm, and then dried in a gear oven at 100° C. for 2 minutes to volatilize the solvent. In this way, a sheet-like molded body C (inner layer; layers excluding the first resin composition layer) having a thickness of 38 μm was formed on the sheet-like molded body A, and a multilayer resin sheet B having a thickness of 40 μm was obtained. The multilayer resin sheet B has a layer structure of sheet-like molded body C / sheet-like molded body A / support.

[0241] [Preparation of Evaluation Substrate] (1) Preparation of Inner Layer Substrate The copper foil on both sides of a glass cloth-based epoxy resin double-sided laminate (copper foil thickness 18 μm, substrate thickness 0.3 mm, size 500 mm × 500 mm, Panasonic "R5715ES") on which an inner layer circuit was formed was etched to produce 25 copper patterns with an L / S of 1 mm / 1 mm and a length of 5 cm, thereby obtaining a textured substrate. The copper surface was then roughened by etching to a depth of 1 μm using a MEC "CZ8100".

[0242] (2) Lamination of multilayer resin sheet to inner layer substrate The obtained multilayer resin sheet B was placed on the substrate surface from the sheet-like molded body C side, and laminated on both sides of the inner layer circuit board using a batch-type vacuum pressure laminator (Nichigo-Morton Co., Ltd., two-stage build-up laminator CVP700) so that the sheet-like molded body C was in contact with the inner layer circuit board. The lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at 100°C and a pressure of 0.74 MPa for 30 seconds. Next, a heat press was performed at 100°C and a pressure of 0.5 MPa for 60 seconds.

[0243] (3) Curing of the Multilayer Resin Sheet The laminated multilayer resin sheet with the support was heated at 100°C for 30 minutes, and then at 170°C for 30 minutes to thermally cure the multilayer resin sheet and form an insulating layer. The obtained laminate sample is referred to as "Laminate Sample D."

[0244] (4) Formation of via holes Hitachi Via Mechanics CO 2 Using a laser processing machine "LC-2E21B / 1C," laminated sample D was drilled to form via holes in the insulating layer. The top diameter (diameter) of the via holes on the insulating layer surface was 50 μm. The drilling conditions were a mask diameter of 1.60 mm, a focus offset value of 0.050, a pulse width of 25 μs, energy of 0.33 mJ / shot (output 0.66 W, frequency 2000 Hz), an aperture of 13, two shots, and burst mode. Next, the support was peeled off from laminated sample D with vias formed therein.

[0245] (5) Desmear Treatment The laminated sample D in which the vias were formed was subjected to a desmear treatment according to the following procedure.

[0246] Swelling treatment: The laminated sample D with vias formed therein was placed in a swelling solution at 60° C. (Swelling Dip Securigant P, manufactured by Atotech Japan, an aqueous solution of diethylene glycol monobutyl ether and sodium hydroxide) and swung for 10 minutes at a swelling temperature of 60° C. Thereafter, the laminated sample D was washed with pure water.

[0247] Roughening treatment: The swollen laminated sample was placed in an oxidant solution ("Concentrate Compact CP" manufactured by Atotech Japan, an aqueous solution containing potassium permanganate at a concentration of approximately 6% and sodium hydroxide at a concentration of approximately 4%) at 80°C, and was shaken at a roughening temperature of 80°C for 20 minutes.

[0248] Neutralization Treatment: After that, the laminate sample was washed with a neutralizing solution (Reduction Securigant P, manufactured by Atotech Japan, aqueous sulfuric acid solution) at 40°C for 10 minutes, and then further washed with pure water. The obtained laminate sample is referred to as "Laminate Sample E".

[0249] [Measurement of surface roughness] For laminated sample E, the Ra value was determined using a non-contact surface roughness meter ("WYKO NT3300" manufactured by Veeco Instruments) in VSI mode with a 50x lens over a measurement range of 121 μm × 92 μm. The average value of 10 randomly selected points was calculated to obtain a measurement value. The surface roughness was determined based on the arithmetic mean roughness (Ra) value according to the following criteria.

[0250] Criteria for arithmetic mean roughness (Ra): ⊚: arithmetic mean roughness (Ra) is less than 30 nm; ◯: arithmetic mean roughness (Ra) is 30 nm or more but less than 50 nm; ×: arithmetic mean roughness (Ra) is 50 nm or more

[0251] [Measurement of Etching Rate] Using an applicator, the obtained resin composition varnish B was applied to the release-treated surface of a PET film (thickness 38 μm), and then dried in a gear oven at 100 ° C. for 2 minutes to volatilize the solvent. In this way, a sheet-like molded product A' having a thickness of 38 μm was obtained on the PET film. Separately, a sheet-like molded product C' having a thickness of 38 μm was obtained on the PET film in the same manner, except that resin composition varnish D was used. Next, the sheet-like molded products A' and C' were each heated at 100 ° C. for 30 minutes, and then at 170 ° C. for 30 minutes to obtain cured products A' and C'. The masses of the obtained cured products A' and C' were each measured.

[0252] Next, the obtained cured bodies A' and C' were subjected to desmear treatment by swelling treatment, roughening treatment, and neutralization treatment in the same manner as described in the above "(5) Desmear treatment". In this way, desmeared cured bodies A" and C" were obtained. The masses of the cured bodies A" and C" after the desmear treatment were measured.

[0253] Using the masses of the obtained cured products A′, C′, A″, and C″, an etching rate RA by desmear treatment of the cured product of the first resin composition layer and an etching rate RD by desmear treatment of the cured product of the resin composition layer that is the outermost layer on the opposite side to the first resin composition layer were calculated based on the following equations.

[0254] Etching rate RA=100×(mass of A'−mass of A″) / mass of A' Etching rate RD=100×(mass of C'−mass of C″) / mass of C'

[0255] <Evaluation of Smear Removability> The periphery of the bottom of the via hole was observed with a scanning electron microscope (SEM), and the maximum smear length from the wall surface of the bottom of the via hole was measured from the obtained image. The smear removability was evaluated according to the following criteria. Evaluation criteria: ○: Maximum smear length is less than 2 μm ×: Maximum smear length is 2 μm or more

[0256] <Evaluation of Cross-Sectional Shape of Via Hole> A cross section of the diameter portion of the via hole was cut out using an FIB and observed using a scanning electron microscope (SEM). From the obtained image, the maximum via diameter R1 in the insulating layer portion derived from the first resin composition layer and the maximum via diameter R2 in the insulating layer portion derived from the layer other than the first resin composition layer were measured. The cross-sectional shape of the via hole was evaluated according to the following criteria.

[0257] Evaluation criteria: ○: R1≧R2 ×: R1<R2

[0258] <Evaluation of film thickness change before and after desmearing> Cross sections of laminate sample D (after thermal curing) and laminate sample E (after desmearing) were cut out using an FIB, and the insulating layers were observed using a scanning electron microscope (SEM). The thicknesses of the insulating layer portions derived from the first resin composition layer were measured from the obtained images. Then, evaluation was performed according to the following criteria based on the difference between the thickness of the insulating layer portion derived from the first resin composition layer in laminate sample D and the thickness of the insulating layer portion derived from the first resin composition layer in laminate sample E.

[0259] Evaluation criteria: ⊚: Thickness difference is less than 0.5 μm ◯: Thickness difference is 0.5 μm or more but less than 1.0 μm ×: Thickness difference is 1.0 μm or more

[0260] Example 2 A sample was produced and evaluated in the same manner as in Example 1, except that the method for forming the inner layer was changed to Formation Method 2 below and the resulting multilayer resin sheet B' was used.

[0261] Formation of inner layer: Formation method 2 - Lamination by lamination Using an applicator, the obtained resin composition varnish D was applied to the release-treated surface of a PET film (thickness 38 μm), and then dried for 2 minutes in a gear oven at 100° C. to volatilize the solvent. In this way, a sheet-like molded product C having a thickness of 38 μm was obtained on the PET film.

[0262] The sheet-like molded body A and the sheet-like molded body C were laminated together with their coated surfaces overlapping each other using a vacuum pressure laminator ("MVLP-500" manufactured by Meiki Seisakusho Co., Ltd.) at a pressure of 0.4 MPa and a temperature of 100°C for 60 seconds to obtain a multilayer resin sheet B'.

[0263] Examples 3 to 5 and Comparative Examples 1 to 3 Samples were prepared and evaluated in the same manner as in Example 1, except that the formulations of the outer layer and inner layer were changed as shown in Table 1.

[0264]

Claims

1. A multilayer resin sheet having two or more resin composition layers consisting of a first resin composition layer which is one outermost layer and a layer other than the first resin composition layer, wherein, when the etching rate by a desmear treatment of a cured product of the first resin composition layer is RA and the etching rate by a desmear treatment of a cured product of the resin composition layer which is the outermost layer opposite the first resin composition layer is RD, RD / RA is 5 or more and less than 100, and the arithmetic mean roughness Ra of the cured product of the first resin composition layer after the desmear treatment is less than 50 nm.

2. A multilayer resin sheet as described in claim 1, wherein when the average particle size (μm) of the inorganic filler in the first resin composition layer is D1 and the average particle size (μm) of the inorganic filler in the layers other than the first resin composition layer is D2, D1 < D2.

3. The multilayer resin sheet according to claim 1, wherein the content of the inorganic filler in the first resin composition layer is 5% by mass or less when the non-volatile components in the first resin composition layer are taken as 100% by mass.

4. The multilayer resin sheet according to claim 1, having an etching rate RA of 0.1% or more and less than 1%.

5. The multilayer resin sheet according to claim 1, wherein when the thickness (μm) of the multilayer resin sheet is T and the thickness (μm) of the first resin composition layer is t, t<(T-t).

6. The multilayer resin sheet according to claim 1, which is used by laminating it on a target material so that the surface opposite to the first resin composition layer is bonded to the target material.

7. The multilayer resin sheet according to claim 1, which is used as an insulating layer for a printed wiring board.

8. A multi-layer resin sheet with a support, comprising the multi-layer resin sheet according to any one of claims 1 to 7 and a support bonded to the first resin composition layer of the multi-layer resin sheet.

9. A method for manufacturing a printed wiring board, comprising the following steps (I) to (IV): (I) a step of laminating the multilayer resin sheet according to any one of claims 1 to 7 on an inner layer substrate so that the surface of the multilayer resin sheet opposite to the first resin composition layer is bonded to the inner layer substrate, (II) a step of curing the multilayer resin sheet to form an insulating layer, (III) a step of forming via holes in the insulating layer with a laser and performing a desmear treatment, and (IV) a step of forming a metal film on the surface of the insulating layer after the desmear treatment.

10. A printed wiring board comprising an insulating layer made of a cured product of the multilayer resin sheet according to any one of claims 1 to 7.

11. A semiconductor device comprising the printed wiring board according to claim 10.

Citation Information

Patent Citations

  • Insulating adhesive sheet and its application

    JP2006045388A

  • Multilayer interconnection board and its manufacturing method

    JP2006202980A

  • Thermosetting resin composition and use thereof

    JP2007056233A

  • Adhesive film, multilayer printed wiring board using the same and method for producing the multilayer printed wiring board

    JP2013035930A

  • Cured body layer, printed wiring board, semiconductor device, resin sheet, method for manufacturing printed wiring board, and method for producing resin sheet

    JP2019218451A