Separation membrane

The separation membrane design with a low load area ratio and polyimide-based functional layer addresses efficiency and cost challenges in acidic gas separation, achieving high retention rates under elevated pressures for spiral membrane elements.

WO2024202568A1PCT designated stage expired Publication Date: 2024-10-03NITTO DENKO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/004215
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-02-07
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Current separation membranes for acidic gases in membrane separation devices, especially spiral membrane elements, face challenges in achieving high efficiency and cost-effectiveness, with existing technologies often requiring complex structures and high operating pressures.

Method used

A separation membrane design featuring a porous support with a low load area ratio, an intermediate layer, and a thin separation functional layer made from polyimide with specific structural units, which maintains a high retention rate of the separation coefficient even under elevated pressures.

Benefits of technology

The membrane achieves a retention rate of 70% or more for the separation coefficient at 2.0 MPa pressure, ensuring efficient separation of acidic gases like carbon dioxide while reducing operational costs and membrane thickness, making it suitable for spiral type membrane elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024004215_03102024_PF_FP_ABST
    Figure JP2024004215_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a novel separation membrane suitable for a membrane separation device (in particular, a spiral membrane element). This separation membrane 10 includes: a separation function layer 1; a porous support body 3 supporting the separation function layer 1; and an intermediate layer 2 arranged between the separation function layer 1 and the porous support body 3. The porous support body 3 includes a surface S1 facing the intermediate layer 2. A load area ratio Smr (c1) of the surface S1 obtained by the following test is less than 80%. Test: three-dimensional analysis is performed with respect to the surface S1 of the porous support body 3 to obtain the load curve defined in JIS B0681-2: 2018. In the load curve, a height c1 is identified, the height such that the difference with a height c0 where the load area ratio is 0% matches the thickness of the intermediate layer 2. A load area ratio corresponding to the height c1 is read and identified as the load area ratio Smr(c1).
Need to check novelty before this filing date? Find Prior Art

Description

Separation membrane

[0001] The present invention relates to a separation membrane.

[0002] Membrane separation has been developed as a method for separating acidic gases such as carbon dioxide from mixed gases. Compared to absorption methods, which separate acidic gases contained in mixed gases by absorbing them into an absorbent, membrane separation methods can efficiently separate acidic gases while reducing operating costs.

[0003] Examples of separation membranes used in membrane separation methods include composite membranes in which a separation functional layer is formed on a porous support, which is typically a laminate in which a microporous layer is laminated on the surface of a nonwoven fabric (see, for example, Patent Document 1).

[0004] Patent No. 6186286

[0005] There is a demand for new separation membranes suitable for membrane separation devices (especially spiral-wound membrane elements).

[0006] The present invention provides a separation membrane comprising: a separation functional layer; a porous support supporting the separation functional layer; and an intermediate layer disposed between the separation functional layer and the porous support, wherein the porous support has a surface S1 facing the intermediate layer, and the area load ratio Smr(c1) of the surface S1 is less than 80% as determined by the following test. Test: Three-dimensional analysis is performed on the surface S1 of the porous support to obtain a load curve as defined in Japanese Industrial Standards (JIS) B0681-2:2018. In the load curve, the height c1, the difference from the height c0 when the area load ratio is 0%, is identified as the thickness of the intermediate layer. The area load ratio corresponding to the height c1 is read and identified as the area load ratio Smr(c1).

[0007] The present invention further provides a separation membrane comprising a separation functional layer, a porous support supporting the separation functional layer, and an intermediate layer disposed between the separation functional layer and the porous support, wherein the thickness of the separation membrane is 130 μm or less, and the retention rate of the separation factor α of the separation membrane when the separation membrane is contacted with nitrogen at a pressure of 2.0 MPa for 5 minutes is 70% or more, wherein the separation factor α is the permeation rate T of nitrogen that permeates the separation membrane when nitrogen at a pressure of 0.6 MPa is supplied to a space adjacent to one side of the separation membrane. N2 (GPU) The permeation rate T of carbon dioxide that permeates the separation membrane when carbon dioxide at a pressure of 0.6 MPa is supplied to the space. CO2 (GPU) ratio T CO2 / T N2 means.

[0008] According to the present invention, a new separation membrane suitable for a membrane separation device (particularly a spiral-wound membrane element) can be provided.

[0009] 1 is a cross-sectional view schematically showing a separation membrane according to one embodiment of the present invention; 2 is a graph for explaining a method for determining the area load ratio Smr(c1); 3 is a schematic cross-sectional view of a membrane separation device provided with the separation membrane of the present invention; 4 is a perspective view schematically showing a modified example of a membrane separation device provided with the separation membrane of the present invention;

[0010] A separation membrane according to a first aspect of the present invention comprises a separation functional layer, a porous support supporting the separation functional layer, and an intermediate layer disposed between the separation functional layer and the porous support, wherein the porous support has a surface S1 facing the intermediate layer, and the area load ratio Smr(c1) of the surface S1 determined by the following test is less than 80%. Test: Three-dimensional analysis is performed on the surface S1 of the porous support to obtain a load curve defined in Japanese Industrial Standards (JIS) B0681-2:2018. In the load curve, the height c1, the difference from the height c0 when the area load ratio is 0%, is determined to be the thickness of the intermediate layer. The area load ratio corresponding to the height c1 is read and determined as the area load ratio Smr(c1).

[0011] In a second aspect of the present invention, for example, in the separation membrane according to the first aspect, the areal load ratio Smr(c1) is 0.04% or more.

[0012] In a third aspect of the present invention, for example, the separation membrane according to the first or second aspect has a thickness of 130 μm or less.

[0013] A separation membrane according to a fourth aspect of the present invention is a separation membrane comprising: a separation functional layer; a porous support supporting the separation functional layer; and an intermediate layer disposed between the separation functional layer and the porous support, wherein the thickness of the separation membrane is 130 μm or less, and the retention rate of the separation factor α of the separation membrane when the separation membrane is contacted with nitrogen at a pressure of 2.0 MPa for 5 minutes is 70% or more. Here, the separation factor α is defined as the permeation rate T of nitrogen that permeates the separation membrane when nitrogen at a pressure of 0.6 MPa is supplied to a space adjacent to one side of the separation membrane. N2 (GPU) The permeation rate T of carbon dioxide that permeates the separation membrane when carbon dioxide at a pressure of 0.6 MPa is supplied to the space. CO2 (GPU) ratio T CO2 / T N2 means.

[0014] In a fifth aspect of the present invention, for example, in the separation membrane according to any one of the first to fourth aspects, the porous support is a fibrous structure.

[0015] In a sixth aspect of the present invention, for example, in the separation membrane according to any one of the first to fifth aspects, the porous support has a thickness of 125 μm or less.

[0016] In a seventh aspect of the present invention, for example, in the separation membrane according to any one of the first to sixth aspects, the ISO air permeability of the porous support is 10.0 × 10 4 μm / (Pa·s) or more.

[0017] In an eighth aspect of the present invention, for example, in the separation membrane according to any one of the first to seventh aspects, the separation functional layer contains polyimide.

[0018] In a ninth aspect of the present invention, for example, in the separation membrane according to the eighth aspect, the polyimide contains a structural unit derived from a tetracarboxylic dianhydride having a six-membered ring acid anhydride structure.

[0019] In a tenth aspect of the present invention, for example, in the separation membrane according to the ninth aspect, the constitutional unit is represented by the following formula (A1). In the formula (A1), R 1a ~R 4a are each independently a hydrogen atom or an optional substituent.

[0020] In an eleventh aspect of the present invention, for example, in the separation membrane according to any one of the first to tenth aspects, the thickness of the separation functional layer is 5.0 μm or less.

[0021] In a twelfth aspect of the present invention, for example, in the separation membrane according to any one of the first to eleventh aspects, the intermediate layer is formed from a pressure-sensitive adhesive composition.

[0022] In a thirteenth aspect of the present invention, for example, in the separation membrane according to the twelfth aspect, the pressure-sensitive adhesive composition contains a silicone-based polymer.

[0023] In a fourteenth aspect of the present invention, for example, in the separation membrane according to any one of the first to thirteenth aspects, the thickness of the intermediate layer is 5.0 μm or less.

[0024] In a fifteenth aspect of the present invention, for example, in the separation membrane according to any one of the first to fourteenth aspects, the peel strength between the intermediate layer and the porous support is 0.25 N / 25 mm or more.

[0025] The present invention will be described in detail below, but the following description is not intended to limit the present invention to a specific embodiment.

[0026] 1 , a separation membrane 10 of this embodiment includes a separation functional layer 1, a porous support 3 supporting the separation functional layer 1, and an intermediate layer 2 disposed between the separation functional layer 1 and the porous support 3. The intermediate layer 2 is preferably in direct contact with both the separation functional layer 1 and the porous support 3.

[0027] The porous support 3 has surfaces S1 and S2 facing each other. Surface S1 faces the intermediate layer 2, and more specifically, is in direct contact with the intermediate layer 2. In this embodiment, the area load ratio Smr(c1) of surface S1 determined by the following test is less than 80%. Test: Three-dimensional analysis is performed on surface S1 of the porous support 3 to obtain a load curve as defined in JIS B0681-2:2018. In the load curve, a height c1 is identified whose difference from the height c0 when the area load ratio is 0% coincides with the thickness of the intermediate layer 2. The area load ratio corresponding to height c1 is read and identified as the area load ratio Smr(c1).

[0028] Specifically, the area load ratio Smr(c1) can be measured by the following method. First, the porous support 3 removed from the separation membrane 10, or the porous support 3 before being used to produce the separation membrane 10, is prepared. This porous support 3 is cut into a size of 1 cm length x 1 cm width to prepare a test piece. The surface S1 of this test piece is observed with a laser microscope. Observation with a laser microscope can be performed under the following conditions. Observation conditions: Light source wavelength: 546 nm Resolution: 0.1 μm Observation range: 600 μm x 600 μm

[0029] Next, three-dimensional analysis is performed using the obtained observation image. The three-dimensional analysis can be performed using LMeye7 software and FinePeak as the analysis algorithm. The three-dimensional analysis can obtain the load curve defined in JIS B0681-2:2018 (FIG. 2). The load curve is a curve showing the relationship between height c and area load ratio Smr in a coordinate system in which the vertical axis is the height c (μm) of the surface S1 (more specifically, the irregularities present on the surface S1) and the horizontal axis is the ratio of the area where the porous support 3 exists in the region above a certain height c (area load ratio Smr (%)).

[0030] Next, as shown in Figure 2, height c0 is identified when the areal bearing ratio Smr is 0% (i.e., the outermost position of the surface S1), and then height c1 is identified whose difference from height c0 coincides with the thickness of the intermediate layer 2. In other words, in Figure 2, the difference |c0-c1| between height c0 and height c1 is the same as the thickness of the intermediate layer 2. The areal bearing ratio corresponding to height c1 can be read and identified as the areal bearing ratio Smr(c1).

[0031] The area load ratio Smr(c1) can be used as an index relating to the pores (openings) present on the surface S1 of the porous support 3. In particular, the lower the area load ratio Smr(c1), the greater the number of pores with relatively large diameters present on the surface S1 of the porous support 3. As an example, when the porous support 3 does not have a microporous layer and is composed only of a fiber structure, the area load ratio Smr(c1) tends to be less than 80%, particularly 50% or less.

[0032] As described above, the area load ratio Smr(c1) of the surface S1 of the porous support 3 is less than 80%, and may be 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, 5.0% or less, 3.0% or less, 1.0% or less, 0.5% or less, or even 0.1% or less. The lower limit of the area load ratio Smr(c1) is, for example, 0.01% or more, and may be 0.04% or more. In particular, when the area load ratio Smr(c1) is 0.04% or more, the peel strength between the porous support 3 and the intermediate layer 2 is sufficiently high, making it easy to produce the separation membrane 10 by the transfer method described below.

[0033] (Separation functional layer) The separation functional layer 1 preferably allows the acidic gas contained in the mixed gas to pass through preferentially, and is typically a dense layer (non-porous layer) in which no pores can be seen when observed at a magnification of 5000 times using a scanning electron microscope (SEM).

[0034] The separation functional layer 1 typically contains a resin. Examples of the resin contained in the separation functional layer 1 include polyether block amide resin, polyamide resin, polyether resin, polyimide resin, cellulose acetate resin, silicone resin, and fluororesin.

[0035] The separation functional layer 1 preferably contains a polyimide, and in particular, preferably contains a polyimide P containing a structural unit A1 derived from a tetracarboxylic dianhydride a1 having a six-membered ring acid anhydride structure S. The polyimide P preferably further contains a structural unit B1 derived from a diamine b1. At least one of the structural units A1 and B1 preferably has at least one functional group f selected from the group consisting of a carboxyl group, a hydroxyl group, a thiol group, and metal salts thereof, and the functional group f preferably has a metal salt (particularly a metal salt of a carboxyl group). In particular, in the polyimide P, it is preferable that the structural unit B1 has the functional group f. The structural unit A1 may or may not have the functional group f.

[0036] The structural unit A1 derived from the tetracarboxylic dianhydride a1 is a structural unit suitable for improving the permeability coefficient and permeation rate of acidic gases that permeate the separation functional layer 1. The tetracarboxylic dianhydride a1 preferably has one or more, preferably two, acid anhydride structures S. The six-membered ring acid anhydride structure S is typically a glutaric anhydride structure represented by the following formula (1):

[0037] The tetracarboxylic dianhydride a1 may further have at least one functional group g selected from the group consisting of a carboxyl group, a hydroxyl group, and a thiol group, or may not have the functional group g. In this specification, the functional group g is the same as the functional group f, except that metal salts are not included as options.

[0038] The tetracarboxylic dianhydride a1 may have a fused ring, and the fused ring may contain an acid anhydride structure S. The fused ring may contain an aromatic ring together with the acid anhydride structure S. The aromatic ring contained in the fused ring may be composed only of carbon atoms, or may be a heteroaromatic ring containing a heteroatom such as an oxygen atom, a nitrogen atom, or a sulfur atom. The aromatic ring may be polycyclic or monocyclic. The number of carbon atoms in the aromatic ring is not particularly limited and is, for example, 4 to 14. Specific examples of the aromatic ring include a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, a furan ring, a pyrrole ring, a pyridine ring, and a thiophene ring.

[0039] The fused ring may or may not have a substituent. The substituent of the fused ring is not particularly limited, and examples thereof include a halogen group and a hydrocarbon group. Examples of the halogen group include a fluoro group, a chloro group, a bromo group, and an iodo group. The number of carbon atoms in the hydrocarbon group is not particularly limited, and is, for example, 1 to 15. Examples of the hydrocarbon group are alkyl groups such as a methyl group, an ethyl group, and a propyl group. The hydrocarbon group may be a halogenated hydrocarbon group in which a hydrogen atom is substituted with a halogen group. When the fused ring has multiple substituents, the multiple substituents may be the same as or different from each other.

[0040] The tetracarboxylic dianhydride a1 is preferably represented by the following formula (a1).

[0041] In formula (a1), R 1a ~R 4a are each independently a hydrogen atom or an arbitrary substituent. The arbitrary substituent is not particularly limited, and examples thereof include a halogen group and a hydrocarbon group. Examples of the halogen group and the hydrocarbon group include those described above.

[0042] In the polyimide P, the structural unit A1 derived from the tetracarboxylic dianhydride a1 is preferably represented by the following formula (A1): The structural unit A1 represented by formula (A1) is derived from the tetracarboxylic dianhydride a1 represented by the above formula (a1). In formula (A1), the nitrogen atom contained in the imide group is derived from the diamine that has reacted with the tetracarboxylic dianhydride a1.

[0043] In formula (A1), R 1a ~R 4a are the same as in formula (a1), and are each independently a hydrogen atom or an arbitrary substituent. Specific examples of the structural unit A1 represented by formula (A1) include the following formula (A1-1).

[0044] In polyimide P, the ratio p1 of the amount of substance of the structural unit A1 to the amount of substances of all structural units A derived from tetracarboxylic dianhydride is, for example, 50 mol% or more, and may be 70 mol% or more, 90 mol% or more, 95 mol% or more, or even 99 mol% or more. Polyimide P may contain only the structural unit A1 as the structural unit A derived from tetracarboxylic dianhydride. However, polyimide P may further contain, in addition to structural unit A1, a structural unit A2 derived from tetracarboxylic dianhydride a2 having a five-membered ring acid anhydride structure. The tetracarboxylic dianhydride a2 is not particularly limited, and examples thereof include pyromellitic acid dianhydride and 4,4'-(hexafluoroisopropylidene)diphthalic anhydride.

[0045] The structural unit B1 derived from diamine b1, particularly the structural unit B1 having the functional group f, is a structural unit suitable for improving the selectivity of acidic gases permeating the separation functional layer 1. Diamine b1 is preferably a compound having two primary amino groups and further having at least one functional group g selected from the group consisting of a carboxyl group, a hydroxyl group, and a thiol group. The number of functional groups g in diamine b1 is not particularly limited and is, for example, 5 or less, preferably 2 or less, and particularly preferably 1. The fewer the number of functional groups g in diamine b1, the more improved the solubility of polyimide P, and the easier it is to apply a desired manufacturing method for separation membrane 10.

[0046] The functional group g has a dissociable proton and can form a salt with a counter cation. In particular, from the viewpoint of easily forming a salt, it is preferable that the diamine b1 has a carboxyl group as the functional group g. It is preferable that the diamine b1 does not have a group having a dissociable proton other than the functional group g, such as a sulfonic acid group. For example, when the diamine b1 does not contain a sulfonic acid group, it is easy to appropriately adjust the solubility of the polyimide P.

[0047] Diamine b1 may further have an aromatic ring. Examples of the aromatic ring include those described above for tetracarboxylic dianhydride a1. In diamine b1, the substituent on the aromatic ring preferably includes a functional group g and a primary amino group. The aromatic ring may have a substituent other than the substituent including the functional group g and the substituent including a primary amino group, or may have no other substituent. The other substituent is not particularly limited, and examples include a halogen group and a hydrocarbon group. Examples of the halogen group and the hydrocarbon group include those described above for tetracarboxylic dianhydride a1. In diamine b1, the other substituent may include a photopolymerizable functional group (e.g., a vinyl group).

[0048] The diamine b1 is preferably represented by the following formula (b1), formula (b2) or formula (b3).

[0049] In formula (b1), R 1b ~R4b are each independently a hydrogen atom or an arbitrary substituent, provided that R 1b ~R 4b At least one selected from the group consisting of is a group containing functional group g, and is preferably functional group g itself. The optional substituent other than the group containing functional group g is not particularly limited, and examples thereof include halogen groups and hydrocarbon groups. Examples of halogen groups and hydrocarbon groups include those described above for tetracarboxylic dianhydride a1.

[0050] In formula (b2), R 5b ~R 12b are each independently a hydrogen atom or an arbitrary substituent, and X 1 is a single bond or any linking group. 5b ~R 12b At least one selected from the group consisting of is a group containing functional group g, and is preferably functional group g itself. The optional substituent other than the group containing functional group g is not particularly limited, and examples thereof include halogen groups and hydrocarbon groups. Examples of halogen groups and hydrocarbon groups include those described above for tetracarboxylic dianhydride a1.

[0051] X in formula (b2) 1 In the formula (I), the optional linking group is, for example, a divalent hydrocarbon group. Examples of the divalent hydrocarbon group include alkylene groups such as methylene, ethylene, propane-1,3-diyl, and propane-2,2-diyl. The divalent hydrocarbon group may be a halogenated hydrocarbon group in which a hydrogen atom is substituted with a halogen group. X 1 may contain a functional group such as an ether group or an ester group in addition to or instead of the divalent hydrocarbon group.

[0052] In formula (b3), R 13b ~R 20b are each independently a hydrogen atom or an arbitrary substituent, and X 2 is a single bond or any linking group. 13b ~R 20bAt least one selected from the group consisting of is a group containing functional group g, and is preferably functional group g itself. The optional substituent other than the group containing functional group g is not particularly limited, and examples thereof include halogen groups and hydrocarbon groups. Examples of halogen groups and hydrocarbon groups include those described above for tetracarboxylic dianhydride a1.

[0053] X in formula (b3) 2 In the formula (I), the optional linking group is, for example, a divalent hydrocarbon group. Examples of the divalent hydrocarbon group include X 1 Examples of the above-mentioned X 2 may contain a functional group such as an ether group or an ester group in addition to or instead of the divalent hydrocarbon group.

[0054] As described above, in the polyimide P, the structural unit B1 derived from the diamine b1 preferably has a functional group f. In particular, the structural unit B1 preferably contains, as the functional group f, a metal salt of a carboxyl group, a metal salt of a hydroxyl group, or a metal salt of a thiol group, and it is particularly preferable that the structural unit B1 contains a metal salt of a carboxyl group.

[0055] The metal contained in the metal salt as functional group f is not particularly limited, and examples thereof include Li, Na, K, Be, Mg, Ca, Ba, Sc, Y, Ti, Zr, V, Cr, Mo, Mn, Fe, Co, Ni, Cu, Ag, Zn, B, Al, Ga, In, Pb, etc., and preferably Mg, Fe, Al, and Ga, and particularly preferably Al. That is, the metal salt as functional group f is preferably an aluminum salt. The metal contained in the metal salt may be Na, Ca, etc.

[0056] In the metal salt as the functional group f, the metal specifically exists as a cation. The valence of the metal (metal cation) contained in the metal salt is, for example, 1 or more, preferably 2 or more, and more preferably 3 or more. For example, the valence of the metal is 2 or 3.

[0057] When the structural unit B1 contains a metal salt as the functional group f, multiple polyimides P can coordinate to the metal cation contained in the metal salt via a functional group such as a carboxyl group. As a result, multiple polyimides P are crosslinked to each other via the metal cation. The formation of such a crosslinked structure tends to suppress physical aging of the polyimide P, thereby suppressing the deterioration of the separation performance of the separation functional layer 1 over time. When the polyimide P contains a metal salt as the functional group f, the separation performance of the separation functional layer 1 also tends to improve. As described below, the metal salt as the functional group f can be formed by exchanging a dissociable proton with a metal cation in the functional group g contained in a polyimide obtained from a monomer group including a tetracarboxylic dianhydride a1 and a diamine b1.

[0058] The structural unit B1 derived from diamine b1 is preferably represented by the following formula (B1), formula (B2), or formula (B3). The structural unit B1 represented by formula (B1) is derived from diamine b1 represented by the above formula (b1). The structural unit B1 represented by formula (B2) is derived from diamine b1 represented by the above formula (b2). The structural unit B1 represented by formula (B3) is derived from diamine b1 represented by the above formula (b3).

[0059] In formula (B1), R 1b ~R 4b are each independently a hydrogen atom or an arbitrary substituent, provided that R 1b ~R 4b At least one selected from the group consisting of is a group containing functional group f, and is preferably functional group f itself. The optional substituent other than the group containing functional group f is not particularly limited, and examples thereof include halogen groups and hydrocarbon groups. Examples of halogen groups and hydrocarbon groups include those described above for tetracarboxylic dianhydride a1.

[0060] Specific examples of the structural unit B1 represented by formula (B1) include the following formulae (B1-1) to (B1-6). In formulae (B1-2), (B1-4), and (B1-6), M represents any metal cation, preferably an Mg ion, an Fe ion, an Al ion, or a Ga ion, and particularly preferably an Al ion. M may also be an Na ion or a Ca ion.

[0061] In formula (B2), R 5b ~R 12b are each independently a hydrogen atom or an arbitrary substituent, and X 1 is a single bond or any linking group. 5b ~R 12b At least one selected from the group consisting of is a group containing functional group f, and is preferably functional group f itself. The optional substituent other than the group containing functional group f is not particularly limited, and examples thereof include halogen groups and hydrocarbon groups. Examples of halogen groups and hydrocarbon groups include those described above for tetracarboxylic dianhydride a1.

[0062] X in formula (B2) 1 In the formula (I), the optional linking group is, for example, a divalent hydrocarbon group. Examples of the divalent hydrocarbon group include those described above. 1 may contain a functional group such as an ether group or an ester group in addition to or instead of the divalent hydrocarbon group.

[0063] Specific examples of the structural unit B1 represented by formula (B2) include the following formulae (B2-1) to (B2-12). In these formulae, M represents any metal cation, preferably an Mg ion, an Fe ion, an Al ion, or a Ga ion, and particularly preferably an Al ion. M may also be a Na ion or a Ca ion.

[0064] In formula (B3), R 13b ~R 20b are each independently a hydrogen atom or an arbitrary substituent, and X 2 is a single bond or any linking group. 13b ~R20b At least one selected from the group consisting of is a group containing functional group f, and is preferably functional group f itself. The optional substituent other than the group containing functional group f is not particularly limited, and examples thereof include halogen groups and hydrocarbon groups. Examples of halogen groups and hydrocarbon groups include those described above for tetracarboxylic dianhydride a1.

[0065] X in formula (B3) 2 In the formula (I), the optional linking group is, for example, a divalent hydrocarbon group. Examples of the divalent hydrocarbon group include those described above. 2 may contain a functional group such as an ether group or an ester group in addition to or instead of the divalent hydrocarbon group.

[0066] Specific examples of the structural unit B1 represented by formula (B3) include the following formulae (B3-1) to (B3-6). In these formulae, M represents any metal cation, preferably an Mg ion, an Fe ion, an Al ion, or a Ga ion, and particularly preferably an Al ion. M may also be a Na ion or a Ca ion.

[0067] In polyimide P, the ratio p2 of the amount of constituent unit B1, particularly the constituent unit B1 having functional group f, to the amount of all constituent units B derived from diamine is, for example, 1 mol% or more, preferably 3 mol% or more. The upper limit of ratio p2 is not particularly limited and may be, for example, 60 mol%, 50 mol%, 40 mol%, 30 mol%, or even 25 mol%. When ratio p2 is low, the solubility of polyimide P improves, and the desired manufacturing method for separation functional layer 1 tends to be easier to apply. Furthermore, in this case, the strength of separation functional layer 1 also tends to be improved. Ratio p2 is preferably 3 to 25 mol%. When ratio p2 is within this range, the separation functional layer 1 tends to have good separation performance.

[0068] Polyimide P may further contain a structural unit B2 derived from diamine b2 having a sulfonyl group (—SO2—). Structural unit B2 is a structural unit suitable for improving the permeation coefficient and permeation rate of acidic gases that permeate through the separation functional layer 1. Diamine b2 is a compound having two primary amino groups in addition to a sulfonyl group. The number of sulfonyl groups in diamine b2 is not particularly limited and may be, for example, 5 or less, preferably 1. Diamine b2 preferably does not contain a group having a dissociable proton, such as the functional group g described above.

[0069] Diamine b2 preferably contains a ring structure having a sulfonyl group, which is typically a thiophene 1,1-dioxide ring or a tetrahydrothiophene 1,1-dioxide ring.

[0070] Diamine b2 may have a fused ring, and the fused ring may contain a ring structure having a sulfonyl group. The fused ring may contain an aromatic ring together with the ring structure having a sulfonyl group. Examples of the aromatic ring include those described above for tetracarboxylic dianhydride a1.

[0071] In diamine b2, the substituent of the fused ring preferably contains a primary amino group. The fused ring may have a substituent other than the substituent containing the primary amino group, or may have no other substituent. The other substituent is not particularly limited, and examples thereof include a halogen group and a hydrocarbon group. Examples of the halogen group and the hydrocarbon group include those described above for tetracarboxylic dianhydride a1.

[0072] The diamine b2 is preferably represented by the following formula (c1).

[0073] In formula (c1), R 1c ~R 6c are each independently a hydrogen atom or an arbitrary substituent. In formula (c1), the arbitrary substituent is, for example, a substituent other than the group containing the functional group g, and specifically, a halogen group, a hydrocarbon group, etc. Examples of the halogen group and the hydrocarbon group include those described above for tetracarboxylic dianhydride a1.

[0074] In the polyimide P, the structural unit B2 derived from the diamine b2 is preferably represented by the following formula (C1): The structural unit B2 represented by formula (C1) is derived from the diamine b2 represented by the above formula (c1).

[0075] In formula (C1), R 1c ~R 6c are each independently a hydrogen atom or an arbitrary substituent. In formula (C1), the arbitrary substituent is, for example, a substituent other than the group containing the functional group f, and more specifically, a halogen group, a hydrocarbon group, etc. Examples of the halogen group and the hydrocarbon group include those described above for the tetracarboxylic dianhydride a1. The structural unit B2 represented by formula (C1) is suitable for improving the rigidity of the polyimide P. A polyimide P with excellent rigidity tends to be able to suppress plasticization of the separation functional layer 1 even when the pressure of the mixed gas to be separated is high.

[0076] Specific examples of the structural unit B2 represented by formula (C1) include the following formulae (C1-1) and (C1-2).

[0077] In the polyimide P, the ratio p3 of the amount of substance of the structural unit B2 to the amount of substances of all structural units B derived from diamine is not particularly limited and may be, for example, 5 mol% or more, 10 mol% or more, 20 mol% or more, 30 mol% or more, or even 40 mol% or more. The upper limit of ratio p3 is not particularly limited and may be, for example, 95 mol%, 90 mol%, 80 mol%, 70 mol%, 60 mol%, or even 50 mol%.

[0078] The polyimide P may further include a structural unit B3 derived from a diamine b3 other than diamines b1 and b2. The diamine b3 is a compound having two primary amino groups and not having the functional group g or a sulfonyl group. The diamine b3 preferably does not include a group having a dissociable proton.

[0079] Diamine b3 may further have an aromatic ring. Examples of the aromatic ring include those described above for tetracarboxylic dianhydride a1. In diamine b3, the substituent on the aromatic ring preferably includes a primary amino group. The aromatic ring may have a substituent other than the substituent including the primary amino group, or may not have any other substituent. Examples of the other substituent include, but are not limited to, a halogen group and a hydrocarbon group. Examples of the halogen group and the hydrocarbon group include those described above for tetracarboxylic dianhydride a1.

[0080] The diamine b3 is preferably represented by the following formula (d1), formula (d2) or formula (d3).

[0081] In formula (d1), R 1d ~R 4d are each independently a hydrogen atom or an arbitrary substituent. In formula (d1), the arbitrary substituent is, for example, a substituent other than the group containing the functional group g and the group containing a sulfonyl group, and more specifically, a halogen group, a hydrocarbon group, etc. Examples of the halogen group and the hydrocarbon group include those described above for tetracarboxylic dianhydride a1.

[0082] In formula (d2), R 5d ~R 8d are each independently a hydrogen atom or an arbitrary substituent. In formula (d2), the arbitrary substituent is, for example, a substituent other than the group containing the functional group g and the group containing a sulfonyl group, and more specifically, a halogen group, a hydrocarbon group, etc. Examples of the halogen group and the hydrocarbon group include those described above for tetracarboxylic dianhydride a1.

[0083] In formula (d3), R 9d ~R 16d are each independently a hydrogen atom or an arbitrary substituent, and X 3is a single bond or an arbitrary linking group. In formula (d3), the arbitrary substituent is, for example, a substituent other than the group containing the functional group g and the group containing a sulfonyl group, and more specifically, a halogen group, a hydrocarbon group, etc. Examples of the halogen group and the hydrocarbon group include those described above for tetracarboxylic dianhydride a1.

[0084] X in formula (d3) 3 In the formula (I), the optional linking group is, for example, a divalent hydrocarbon group. Examples of the divalent hydrocarbon group include those described above. 3 In the formula (I), the divalent hydrocarbon group may further have an aromatic ring. Examples of the aromatic ring include those described above for the tetracarboxylic dianhydride a1. 3 The divalent hydrocarbon group in X may be a fluorenediyl group. 3 may contain a functional group such as an ether group or an ester group in addition to or instead of the divalent hydrocarbon group.

[0085] The structural unit B3 derived from diamine b3 is preferably represented by the following formula (D1), formula (D2), or formula (D3). The structural unit B3 represented by formula (D1) is derived from diamine b3 represented by formula (d1) above. The structural unit B3 represented by formula (D2) is derived from diamine b3 represented by formula (d2) above. The structural unit B3 represented by formula (D3) is derived from diamine b3 represented by formula (d3) above.

[0086] In formula (D1), R 1d ~R 4d are each independently a hydrogen atom or an arbitrary substituent. In formula (D1), the arbitrary substituent is, for example, a substituent other than a group containing the above-mentioned functional group f, and more specifically, a halogen group, a hydrocarbon group, etc. Examples of the halogen group and the hydrocarbon group include those described above for the tetracarboxylic dianhydride a1. Specific examples of the structural unit B3 represented by formula (D1) include formula (D1-1) below.

[0087] In formula (D2), R 5d ~R 8dare each independently a hydrogen atom or an arbitrary substituent. In formula (D2), the arbitrary substituent is, for example, a substituent other than a group containing the above-mentioned functional group f, and more specifically, a halogen group, a hydrocarbon group, etc. Examples of the halogen group and the hydrocarbon group include those described above for the tetracarboxylic dianhydride a1. Specific examples of the structural unit B3 represented by formula (D2) include formula (D2-1) below.

[0088] In formula (D3), R 9d ~R 16d are each independently a hydrogen atom or an arbitrary substituent, and X 3 is a single bond or an arbitrary linking group. In formula (D3), the arbitrary substituent is, for example, a substituent other than the group containing the functional group f, and specifically, a halogen group, a hydrocarbon group, etc. Examples of the halogen group and the hydrocarbon group include those described above for tetracarboxylic dianhydride a1. X in formula (D3) 3 In the formula (I), the optional linking group is, for example, a divalent hydrocarbon group. Examples of the divalent hydrocarbon group include those described above. 3 may contain a functional group such as an ether group or an ester group in addition to or instead of the divalent hydrocarbon group. Specific examples of the structural unit B3 represented by formula (D3) include the following formulae (D3-1) to (D3-3).

[0089] In the polyimide P, the ratio p4 of the amount of substance of the structural unit B3 to the amount of substances of all structural units B derived from diamines is not particularly limited and may be, for example, 5 mol% or more, 10 mol% or more, 20 mol% or more, 30 mol% or more, or even 40 mol% or more. The upper limit of ratio p4 is not particularly limited and may be, for example, 95 mol%, 90 mol%, 80 mol%, 70 mol%, 60 mol%, or even 50 mol%.

[0090] In polyimide P, structural units A derived from tetracarboxylic dianhydride and structural units B derived from diamine are arranged alternately. Examples of combinations of adjacent structural units A and B in polyimide P include those represented by the following formulae (A1-B1), (A1-B2), (A1-C1), and (A1-D1). In these formulae, R 1a ~R 4a , R 1b ~R 12b , R 1c ~R 6c and R 1d ~R 4d is the same as described above for formula (A1), formula (B1), formula (B2), formula (C1) and formula (D1).

[0091] The weight average molecular weight (Mw) of polyimide P is, for example, 30,000 or more, preferably 50,000 or more, and more preferably 75,000 or more, from the viewpoint of the mechanical strength of the separation functional layer 1. The upper limit of the weight average molecular weight of polyimide P is not particularly limited and is, for example, 1,000,000. The weight average molecular weight of polyimide P can be calculated from the obtained chromatogram (chart) by measuring the molecular weight distribution of polyimide P using a gel permeation chromatograph (GPC) equipped with a differential refractive index detector (RID) using a calibration curve based on standard polystyrene.

[0092] The content of polyimide P in the separation functional layer 1 is, for example, 50 wt % or more, and may be 60 wt % or more, 70 wt % or more, 80 wt % or more, 90 wt % or more, or even 95 wt % or more. The separation functional layer 1 may be composed essentially of polyimide P only.

[0093] The separation functional layer 1 may further contain other components besides polyimide P. Examples of the other components include a filler. Examples of the filler include those exemplified for the intermediate layer 2 described below. In the separation functional layer 1, the filler is preferably dispersed in a matrix containing polyimide P. The fillers may be separated from each other within the matrix, or may be partially aggregated.

[0094] The thickness of the separation functional layer 1 is, for example, 10 μm or less, and may be 8.0 μm or less, 5.0 μm or less, 4.0 μm or less, 3.0 μm or less, or even 2.0 μm or less. The thickness of the separation functional layer 1 may be 0.05 μm or more, or may be 0.1 μm or more.

[0095] (Intermediate layer) The intermediate layer 2 is preferably formed from a pressure-sensitive adhesive composition, particularly a pressure-sensitive adhesive composition containing a silicone-based polymer. The silicone-based polymer refers to a polymer having a structural unit containing a siloxane bond. In this specification, a pressure-sensitive adhesive composition containing a silicone-based polymer may be referred to as a "silicone-based pressure-sensitive adhesive."

[0096] Examples of silicone-based adhesives include peroxide-crosslinking silicone-based adhesives, addition reaction silicone-based adhesives, and active energy ray-curing silicone-based adhesives. Peroxide-crosslinking silicone-based adhesives contain an organic peroxide (e.g., benzoyl peroxide). This organic peroxide causes radical crosslinking. Examples of addition reaction silicone-based adhesives include hydrosilylation silicone-based adhesives. Hydrosilylation silicone-based adhesives contain a SiH group-containing siloxane crosslinker and a platinum-based catalyst. Crosslinking occurs through a hydrosilylation reaction using this platinum-based catalyst. Active energy ray-curing silicone-based adhesives undergo a crosslinking reaction in the presence of light such as ultraviolet light or an electron beam. In particular, addition reaction silicone-based adhesives, such as hydrosilylation silicone-based adhesives, are preferred in terms of their tendency to leave residues in the intermediate layer 2, their ability to react at low temperatures, and their reaction speed.

[0097] The silicone-based adhesive preferably contains a silicone resin component and a silicone gum component as the silicone-based polymer, since the adhesiveness, releasability, and cohesiveness can be easily controlled.

[0098] The silicone resin component is not particularly limited, but is preferably a branched polyorganosiloxane containing hydroxyl groups bonded to silicon atoms in the molecule, and 1 / 2 ), Q units (SiO2), T units (RSiO 3 / 2It is more preferable that the silicone resin component is a polyorganosiloxane having at least one unit selected from the group consisting of M units (RSiO) and D units (RSiO). In the above units, R is, independently of each other, a monovalent hydrocarbon group or a hydroxyl group. Examples of monovalent hydrocarbon groups include alkyl groups (e.g., methyl, ethyl, propyl, etc.), alkenyl groups (e.g., vinyl, etc.), and aryl groups (e.g., phenyl, etc.). In particular, the silicone resin component is preferably a polyorganosiloxane having at least one unit selected from the group consisting of M units (RSiO). 1 / 2 It is preferable that the silicone resin component is an MQ resin composed of a siloxane unit (SiO2) and a Q unit (SiO2). The silicone resin component may be used alone or in combination of two or more kinds.

[0099] The silicone gum component is not particularly limited, but is preferably a linear polyorganosiloxane represented by the following formula (2).

[0100] In formula (2), R's are each independently a methyl group, a phenyl group, or an alkenyl group, and n is an integer of 100 to 10,000. The silicone gum component may be used alone or in combination of two or more types.

[0101] In the peroxide-crosslinking silicone-based pressure-sensitive adhesive, the silicone gum component preferably contains a methyl group. In the peroxide-crosslinking silicone-based pressure-sensitive adhesive, the methyl group of the silicone gum component is radically crosslinked. In the hydrosilylation-type silicone-based pressure-sensitive adhesive, the silicone gum component preferably contains an alkenyl group, particularly a vinyl group. In the hydrosilylation-type silicone-based pressure-sensitive adhesive, the alkenyl group of the silicone gum component is crosslinked by a hydrosilylation reaction.

[0102] The pressure-sensitive adhesive composition (silicone-based pressure-sensitive adhesive) may contain additives other than the silicone resin component and the silicone gum component. Examples of additives include materials for promoting crosslinking reactions (organic peroxides, SiH group-containing siloxane crosslinkers, platinum-based catalysts, etc.), adhesion improvers (e.g., X-92-185 manufactured by Shin-Etsu Chemical Co., Ltd.), silane coupling agents, fillers, plasticizers, antioxidants, antistatic agents, colorants (pigments, dyes), and fillers described below. The additives may be used alone or in combination of two or more.

[0103] The pressure-sensitive adhesive composition (silicone-based pressure-sensitive adhesive) may further contain an organic solvent (for example, toluene, xylene, etc.).

[0104] Specific examples of pressure-sensitive adhesive compositions (silicone-based pressure-sensitive adhesives) include "KR-3700," "KR-3701," and "KR-3704" manufactured by Shin-Etsu Chemical Co., Ltd. These commercially available products are provided as products containing both a silicone gum component and a silicone resin component. The silicone-based pressure-sensitive adhesive may contain a mixture of these commercially available products.

[0105] As described above, the intermediate layer 2 is preferably formed from a pressure-sensitive adhesive composition, particularly a pressure-sensitive adhesive composition containing a silicone-based polymer (a silicone-based pressure-sensitive adhesive). The intermediate layer 2 formed from a silicone-based pressure-sensitive adhesive preferably contains a crosslinked silicone-based polymer. The content of the crosslinked silicone-based polymer in the intermediate layer 2 is not particularly limited, and is, for example, 60 wt % or more, preferably 70 wt % or more, and more preferably 90 wt % or more. The intermediate layer 2 may be substantially composed of the crosslinked silicone-based polymer.

[0106] The intermediate layer 2 may further contain the additives described above, particularly a filler. An intermediate layer 2 containing a filler is suitable for improving the permeation rate of acidic gases through the separation membrane 10. The filler may contain an inorganic material or an organic material. Examples of inorganic materials contained in the filler include zeolite, silica, titania, and alumina. Examples of organic materials include (meth)acrylic polymers. In this specification, "(meth)acrylic polymer" refers to an acrylic polymer and / or a methacrylic polymer.

[0107] The filler may include a metal-organic framework (MOF). The metal-organic framework is also called a porous coordination polymer (PCP). The metal-organic framework preferably includes metal ions and organic ligands. Examples of the metal ions include Cu ions and Zn ions. The organic ligand preferably includes an aromatic ring. Examples of the aromatic ring included in the organic ligand include a benzene ring and an imidazole ring. Examples of the organic ligand include trimesic acid and 2-methylimidazole. Specific examples of the metal-organic framework include HKUST-1 and ZIF-8.

[0108] The filler is typically in the form of particles. In this specification, the term "particulate" includes spherical, ellipsoidal, scaly, fibrous, and the like.

[0109] The average particle diameter of the filler is not particularly limited and may be, for example, 5 μm or less, 1 μm or less, 800 nm or less, 600 nm or less, 500 nm or less, 400 nm or less, 300 nm or less, 200 nm or less, or even 100 nm or less. The lower limit of the average particle diameter of the filler is, for example, 1 nm. The average particle diameter of the filler can be determined by the following method. First, a cross section of the intermediate layer 2 is observed using a transmission electron microscope. In the obtained electron microscope image, the area of ​​a specific filler is calculated by image processing. The diameter of a circle having the same area as the calculated area is regarded as the particle diameter of that specific filler (particle diameter). The particle diameters of an arbitrary number (at least 50) of fillers are calculated, and the average of the calculated values ​​is regarded as the average particle diameter of the filler.

[0110] The filler content in the intermediate layer 2 is, for example, 40 wt % or less, and may be 30 wt % or less, 20 wt % or less, or even 10 wt % or less, from the viewpoint of suppressing an increase in the storage modulus of the intermediate layer 2. The lower limit of the filler content in the intermediate layer 2 is not particularly limited, but is, for example, 1 wt % from the viewpoint of improving the permeation rate of acidic gases.

[0111] The intermediate layer 2 formed from the pressure-sensitive adhesive composition tends to have a low storage modulus. For example, the storage modulus of the intermediate layer 2 at 25° C. is, for example, 1.0×10 5 Pa or less, preferably 0.95×10 5 Pa or less, and 5 Pa or less, and may be 0.85 × 10 5 The lower the storage modulus of the intermediate layer 2, the greater the adhesive strength between the intermediate layer 2 and the porous support 3. The storage modulus of the intermediate layer 2 at 25° C. may be 0.1×10 5 It is preferable that the pressure is 0.05 Pa or more.

[0112] The storage modulus of the intermediate layer 2 at 25°C can be determined by the following method. First, a measurement sample made of the material that constitutes the intermediate layer 2 is prepared. The measurement sample is disc-shaped. The measurement sample has a bottom diameter of 8 mm and a thickness of 2 mm. The measurement sample may be prepared by preparing multiple intermediate layers 2, laminating them, and punching them into a disc-shaped laminate. Next, dynamic viscoelasticity measurement is performed on the measurement sample. For the dynamic viscoelasticity measurement, an Advanced Rheometric Expansion System (ARES) manufactured by Rheometric Scientific can be used. The storage modulus of the intermediate layer 2 at 25°C can be determined from the results of the dynamic viscoelasticity measurement. The conditions for the dynamic viscoelasticity measurement are as follows: Measurement conditions Frequency: 1 Hz Deformation mode: Torsion Measurement temperature: -70°C to 150°C Heating rate: 5°C / min

[0113] The thickness of the intermediate layer 2 is, for example, 10 μm or less, and may be 8.0 μm or less, 5.0 μm or less, 4.0 μm or less, 3.0 μm or less, or even 2.0 μm or less. The thickness of the intermediate layer 2 may be 0.05 μm or more, 0.1 μm or more, or even 0.5 μm or more.

[0114] (Porous Support) In this embodiment, the porous support 3 preferably has only a main body portion and does not have a microporous layer made of a polymer or the like. The porous support 3 may be composed of only a single material. The porous support 3 is preferably a fibrous structure such as a woven fabric, a nonwoven fabric, a net, or a mesh, and is typically a nonwoven fabric. Examples of fibers contained in the fibrous structure include natural fibers such as wood pulp, cotton, and hemp (e.g., Manila hemp); and chemical fibers (synthetic fibers) such as polyester fibers, polyphenylene sulfide (PPS) fibers, rayon, vinylon, acetate fibers, polyvinyl alcohol (PVA) fibers, polyamide fibers, polyolefin fibers, and polyurethane fibers. The porous support 3 is preferably a nonwoven fabric made of polyester fibers such as polyethylene terephthalate (PET) fibers, or a nonwoven fabric made of PPS fibers. In this embodiment, the intermediate layer 2 is preferably in direct contact with the fibrous structure (specifically, the nonwoven fabric).

[0115] In another aspect, the present invention provides a separation membrane (10) comprising: a separation functional layer (1); a porous support (3) supporting the separation functional layer (1); and an intermediate layer (2) disposed between the separation functional layer (1) and the porous support (3) and in direct contact with the porous support (3), wherein the porous support (3) is a fibrous structure.

[0116] As described above, in this embodiment, the porous support 3 does not have, for example, a microporous layer and tends to have a small thickness. The thickness of the porous support 3 is, for example, 200 μm or less, and may be 150 μm or less, 125 μm or less, 110 μm or less, 100 μm or less, 80 μm or less, or even 60 μm or less. The lower limit of the thickness of the porous support 3 may be, for example, 10 μm or more, 30 μm or more, or even 50 μm or more.

[0117] In this embodiment, the porous support 3 has a low area load ratio Smr(c1) of the surface S1, and therefore tends to have high air permeability by itself. For example, the ISO air permeability of the porous support 3 is, for example, 5.0 × 10 4 μm / (Pa s) or more, and 10.0 × 10 4 μm / (Pa・s) or more, 20.0×104 μm / (Pa・s) or more, 30.0×10 4 μm / (Pa・s) or more, 40.0×10 4 μm / (Pa・s) or more, 50.0×10 4 μm / (Pa・s) or more, 70.0×10 4 μm / (Pa s) or more, and even 100.0 × 10 4 The upper limit of the ISO air permeability of the porous support 3 is not particularly limited, and may be, for example, 1000.0 × 10 4 The ISO air permeability of the porous support body 3 can be measured in accordance with the Oken type testing machine method specified in JIS P8117:2009.

[0118] In this embodiment, it is preferable that the intermediate layer 2 and the porous support 3 are bonded with sufficient strength. For example, the peel strength between the intermediate layer 2 and the porous support 3 may be, for example, 0.25 N / 25 mm or more, 0.50 N / 25 mm or more, 0.75 N / 25 mm or more, 1.00 N / 25 mm or more, 1.25 N / 25 mm or more, 1.50 N / 25 mm or more, 1.75 N / 25 mm or more, or even 2.00 N / 25 mm or more. The upper limit of this peel strength is not particularly limited, and is, for example, 10.0 N / 25 mm or less.

[0119] The peel strength between the intermediate layer 2 and the porous support 3 can be measured by the following method. First, the intermediate layer 2 is prepared on an evaluation sheet (DIAFOIL T100-50, manufactured by Mitsubishi Plastics, Inc., thickness: 50 μm). The intermediate layer 2 can be prepared by the method described below. Next, the entire surface of the intermediate layer 2 is superimposed on the porous support 3, and they are pressed together by rolling a 2 kg roller back and forth once. This forms a laminate having the evaluation sheet, intermediate layer 2, and porous support 3 in this order. This laminate is cut into a width of 25 mm and a length of 100 mm to prepare a test piece. Next, the entire surface of the porous support 3 provided on the test piece is superimposed on a polyethylene terephthalate film via double-sided adhesive tape (No. 500, manufactured by Nitto Denko Corporation), and they are pressed together by rolling a 2 kg roller back and forth once. Next, using a commercially available tensile tester, the porous support 3 together with the film is peeled off from the intermediate layer 2 at a peel angle of 180° and a peel rate of 100 mm / min. The peel force at this time can be regarded as the peel strength between the intermediate layer 2 and the porous support 3. The above measurement is carried out in an atmosphere of 23°C.

[0120] (Method for manufacturing separation membrane) The separation membrane 10 of this embodiment can be manufactured by the following method: First, a coating liquid containing the material of the separation functional layer 1 is applied onto a substrate and dried to form the separation functional layer 1.

[0121] In a preferred embodiment, the coating liquid contains a polyimide Q having at least one functional group g selected from the group consisting of a carboxyl group, a hydroxyl group, and a thiol group, and a metal-containing compound M. In this embodiment, the polyimide Q is a precursor of the polyimide P, and the polyimide P can be formed from the polyimide Q by exchanging the dissociative proton of the functional group g with a metal cation. As will be described later, this coating liquid can form a polyimide P having a metal salt as the functional group f.

[0122] Polyimide Q can be prepared by the following method: First, a diamine group including the diamine b1 is dissolved in a solvent to obtain a solution. Examples of the solvent include polar organic solvents such as N-methyl-2-pyrrolidone and 1,3-dioxolane.

[0123] Next, the tetracarboxylic dianhydrides including the tetracarboxylic dianhydride a1 are gradually added to the resulting solution. This causes the tetracarboxylic dianhydride a1 to react with the monomers including the diamine b1 to form a polyamic acid. The addition of the tetracarboxylic dianhydrides is preferably carried out under stirring in a heated environment of 140°C or higher for 3 to 20 hours.

[0124] Next, polyamic acid is imidized to obtain polyimide Q. Examples of the imidization method include chemical imidization and thermal imidization. The chemical imidization method is a method in which polyamic acid is imidized, for example, at room temperature using a dehydration condensation agent. Examples of the dehydration condensation agent include acetic anhydride, pyridine, and triethylamine. The thermal imidization method is a method in which polyamic acid is imidized by heat treatment. The temperature of the heat treatment is, for example, 180°C or higher.

[0125] The content of Polyimide Q in the coating liquid can be adjusted appropriately depending on the solubility of Polyimide Q, and is, for example, 1 wt % to 30 wt %. In the coating liquid, the ratio of the weight of Polyimide Q to the total weight of Polyimide Q and the solvent is, for example, 1 wt % to 30 wt %.

[0126] Examples of the metal contained in compound M include those metals contained in the metal salt as functional group f described above. In compound M, the metal is preferably present as a cation. Examples of compound M include a metal complex having a metal and a ligand coordinated to the metal, and an inorganic salt containing a metal. Compound M preferably contains a metal complex.

[0127] In the metal complex, the ligand is preferably volatile. As an example, the boiling point of the ligand may be 20°C to 260°C under atmospheric pressure (101.325 kPa). A volatile ligand is likely to volatilize when the coating film described below is dried, and is unlikely to remain in the separation functional layer 1. The ligand does not have to be volatile. In this case, the ligand can be easily removed from the separation functional layer 1 by performing a cleaning operation after the separation functional layer 1 is formed.

[0128] In metal complexes, the ligand is typically an organic ligand having a functional group for coordinating to the metal. The number of carbon atoms in the organic ligand is not particularly limited and may be, for example, 1 to 10. Examples of functional groups contained in the organic ligand include carbonyl groups such as ketone groups. The number of functional groups contained in the organic ligand may be, for example, 1 or more, and may be 2 or more. Specific examples of organic ligands include acetylacetonate (acac). Specific examples of metal complexes include Al(acac)3, Fe(acac)2, Ga(acac)3, and Mg(acac)2.

[0129] Examples of inorganic salts include chlorides, nitrates, and sulfates, and more specifically, LiCl, NaCl, KCl, AgNO, MgCl, CaCl, BaCl, NiCl, ZnCl, CuCl, Pb(NO), Al(NO), Fe(SO), Ga(NO), Fe(NO), and Mg(NO).

[0130] In the coating solution, the ratio of the weight of compound M to the weight of polyimide Q can be appropriately adjusted depending on the composition of polyimide Q, and may be, for example, 1 to 20 wt %, or may be 1 to 10 wt %. In the coating solution, the ratio of the substance amount of compound M to the substance amount of functional group g contained in polyimide Q is not particularly limited, and is, for example, 2.0 or more.

[0131] The coating liquid may further contain a ligand when it contains a metal complex as compound M. In the coating liquid, the weight ratio of the ligand to the weight of polyimide Q can be appropriately adjusted depending on the content of polyimide Q and the metal complex, and may be, for example, 1 to 20 wt %, or may be 1 to 10 wt %.

[0132] The coating liquid preferably further contains a solvent. The solvent is typically a good solvent capable of dissolving Polyimide Q. The solvent preferably contains at least one selected from the group consisting of amide compounds and lactone compounds, and more preferably contains an amide compound. Examples of amide compounds include N,N-dimethylformamide (DMF), N-methyl-2-pyrrolidone (NMP), and N,N-dimethylacetamide (DMAc). Examples of lactone compounds include γ-butyrolactone.

[0133] The content of the solvent in the coating liquid is, for example, 30 wt % to 95 wt %. In the coating liquid, the ratio of the weight of the solvent to the total weight of the Polyimide Q and the solvent is, for example, 30 wt % to 95 wt %.

[0134] The coating liquid is not limited to the above-mentioned composition. In another preferred embodiment, the coating liquid contains polyimide P instead of the polyimide Q and compound M. In this embodiment, polyimide P preferably has at least one functional group f selected from the group consisting of a carboxyl group, a hydroxyl group, a thiol group, and metal salts thereof.

[0135] The substrate is typically a release liner. Examples of the substrate include films containing resin; paper; and sheets containing metal materials such as aluminum and stainless steel. Sheets containing metal materials tend to have high heat resistance. The substrate is preferably a film containing resin because it has excellent surface smoothness. In the substrate, examples of the polymer contained in the resin include polyolefins such as polyethylene, polypropylene, polybutene, polybutadiene, and polymethylpentene; polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyvinyl chloride, vinyl chloride copolymers; polyurethanes; ethylene-vinyl acetate copolymers; and polyimides, with polyimides being preferred.

[0136] The surface of the substrate may be subjected to a release treatment. The release treatment can be carried out by applying a release treatment agent to the surface of the substrate. Examples of the release treatment agent include silicone-based release treatment agents, long-chain alkyl-based release treatment agents, fluorine-based release treatment agents, and molybdenum sulfide-based release treatment agents. The release treatment agents may be used alone or in combination of two or more. The substrate is preferably a polyimide film that has been subjected to a release treatment.

[0137] The thickness of the substrate is not particularly limited, and is, for example, 5 to 100 μm, and preferably 10 to 50 μm.

[0138] Before applying the coating liquid, the substrate may be subjected to a surface modification treatment. When the substrate has been subjected to a release treatment, the surface modification treatment may be performed on the surface of the substrate that has been subjected to the release treatment. Examples of the surface modification treatment include corona treatment, plasma treatment, excimer treatment, and flame treatment, and corona treatment is preferred.

[0139] The surface modification treatment can be carried out by irradiating the surface of the substrate with active energy rays. Specific examples of active energy rays include electron beams, ion beams, plasma beams, and ultraviolet rays. When corona treatment is performed as the surface modification treatment, the discharge amount is, for example, 0.1 kW min / m 2 The upper limit of the discharge amount is not particularly limited, and may be, for example, 10 kW min / m 2 is.

[0140] The method for applying the coating liquid to the substrate is not particularly limited, and for example, spin coating, dip coating, slot die coating, etc. may be used. The coating liquid may be applied to the substrate using an applicator, a wire bar, etc. The coating liquid may be applied to the surface of a substrate that has been subjected to a release treatment or a surface modification treatment.

[0141] The coating liquid is applied to the substrate to form a coating film. The thickness of the coating film can be adjusted appropriately depending on the desired thickness of the separation functional layer 1, and is, for example, 1 μm to 100 μm.

[0142] In this embodiment, the separation functional layer 1 can be obtained by drying the coating film. The drying conditions for the coating film are not particularly limited, and for example, the drying temperature is 50°C to 200°C and the drying time is 1 minute to 10 hours. The coating film can be dried using a heater or the like. As an example, the coating film may be dried by passing it through a heating unit equipped with a heater. The coating film may be dried by passing it through multiple heating units. The set temperatures of the multiple heating units may be the same or different from each other.

[0143] When the coating solution contains a polyimide Q having a functional group g and a compound M having a metal, when the coating film is dried, the dissociative protons contained in the functional group g of the polyimide Q are exchanged with the metal (metal cation) of the compound M. In particular, when the compound M is a metal complex and the ligand contained in the metal complex is volatile, the volatilization of the ligand during drying tends to promote the exchange of the dissociative protons of the functional group g with the metal of the compound M. The exchange of the dissociative protons of the functional group g with the metal of the compound M forms a metal salt of the functional group g, and polyimide P is formed from the polyimide Q. In the separation functional layer 1 obtained by this method, multiple polyimide P molecules are usually crosslinked with each other via metal cations. Due to this crosslinked structure, the separation functional layer 1 tends to have high solvent resistance.

[0144] The exchange of the dissociative protons contained in the functional group g of the polyimide Q with the metal of the compound M may be performed after the formation of the separation functional layer 1. For example, a coating liquid containing the above-described polyimide Q and a solvent is applied to a substrate and dried to form the separation functional layer 1. The separation functional layer 1 may be immersed in a solution containing the above-described compound M to exchange the dissociative protons of the functional group g with the metal of the compound M. The solution containing the compound M is preferably an aqueous solution containing the above-described inorganic salt. The concentration of the inorganic salt in the aqueous solution is not particularly limited, and is, for example, 0.01 to 1 mol / L. The conditions for immersing the separation functional layer 1 in the solution containing the compound M are not particularly limited, and the immersion may be performed at room temperature for 1 to 48 hours. After immersion in the above-described solution, the separation functional layer 1 may be further washed with water or dried. The drying may be performed at a temperature of 150°C or less for 1 to 24 hours.

[0145] The method for forming the separation functional layer 1 is not limited to the above-mentioned method. The separation functional layer 1 may be formed by applying a coating liquid containing the above-mentioned polyimide P and a solvent onto a substrate and drying it. Alternatively, the separation functional layer 1 may be produced by applying a coating liquid containing polyamic acid, which is a precursor of polyimide P, onto a substrate and imidizing the polyamic acid to form polyimide P.

[0146] The produced separation functional layer 1 may be further subjected to a heat treatment (annealing treatment). This treatment improves the separation performance of the separation functional layer 1 and also tends to suppress deterioration over time of the separation performance of the separation functional layer 1. This treatment also makes it possible to obtain a separation functional layer 1 that contains almost no residual solvent by sufficiently volatilizing the solvent.

[0147] The temperature of the heat treatment may be, for example, higher than 200°C, 230°C or higher, or even 250°C or higher. The upper limit of the temperature of the heat treatment is not particularly limited, and may be, for example, 350°C or lower, or 300°C or lower. The time of the heat treatment is, for example, 1 minute or longer, or may be 10 minutes or longer, or 30 minutes or longer. The upper limit of the time of the heat treatment is not particularly limited, and may be, for example, 24 hours or shorter.

[0148] Next, a coating liquid containing the material for intermediate layer 2 is applied onto the separation functional layer 1 and then dried to form intermediate layer 2. The coating liquid containing the material for intermediate layer 2 is typically the above-mentioned adhesive composition. Examples of methods for applying the coating liquid include the methods described above for separation functional layer 1. A coating film is formed by applying the coating liquid onto the separation functional layer 1. The coating film is then dried to form intermediate layer 2. The coating film can be dried under heating conditions. For example, if the coating liquid is an addition reaction type silicone-based adhesive, the coating film may be dried by heating at 100 to 130°C. Under the above heating conditions, it is preferable that the crosslinking reaction of the silicone-based polymer proceeds as the coating film dries, forming a crosslinked product of the silicone-based polymer. The heating time for the coating film is, for example, 1 minute or more, and may be 5 minutes or more. By drying the coating film, a laminate having a substrate, separation functional layer 1, and intermediate layer 2 in this order can be obtained. In this laminate, intermediate layer 2 is exposed to the outside of the laminate.

[0149] Next, the intermediate layer 2 of the above laminate is bonded to the porous support 3. There are no particular limitations on the method for bonding the intermediate layer 2 to the porous support 3, and any known method can be used. For example, the intermediate layer 2 can be bonded to the porous support 3 by overlapping the intermediate layer 2 and the porous support 3 and pressing them together by moving a roller back and forth. The separation membrane 10 can be obtained by removing the substrate from the resulting laminate.

[0150] Conventionally, separation membranes are produced by applying a coating solution containing an intermediate layer material onto a porous support to form an intermediate layer, and then forming a separation functional layer on the intermediate layer (see, for example, Patent Document 1). In this method, the pores on the surface of the porous support on the intermediate layer side must have a small pore size to prevent the coating solution from penetrating into the porous support. Therefore, this method typically uses a porous support in which a microporous layer is laminated on the surface of a nonwoven fabric. However, this porous support is thicker due to the presence of the microporous layer.

[0151] According to the inventors' investigations, the transfer method of transferring a separation functional layer and an intermediate layer to a porous support does not require adjusting the pore size of the surface pores of the porous support on the intermediate layer side to be small, and does not require the use of a porous support having a microporous layer. In this embodiment, by using a porous support 3 without a microporous layer, the thickness (total membrane thickness) of the separation membrane 10 can be adjusted to be small. A separation membrane 10 with a small thickness can easily increase the membrane area of ​​the separation membrane 10 that can be installed in a membrane separation device (particularly a spiral membrane element). Thus, the separation membrane 10 of this embodiment can be said to be suitable for a membrane separation device (particularly a spiral membrane element). Furthermore, by using a porous support 3 without a microporous layer, the separation membrane 10 tends to be produced inexpensively.

[0152] (Shape of Separation Membrane) In this embodiment, the separation membrane 10 is typically a flat membrane. However, the separation membrane 10 may have a shape other than a flat membrane, and may be a hollow fiber membrane.

[0153] In this embodiment, the thickness of the porous support 3 is small, and the thickness of the separation membrane 10 also tends to be small. The thickness of the separation membrane 10 is, for example, 135 μm or less, and may be 130 μm or less, 120 μm or less, 110 μm or less, 100 μm or less, 90 μm or less, 80 μm or less, or even 70 μm or less. The lower limit of the thickness of the separation membrane 10 is, for example, 20 μm or more, and may be 30 μm or more, 40 μm or more, or even 50 μm or more.

[0154] (Characteristics of Separation Membrane) The separation membrane 10 tends to have high pressure resistance due to the inclusion of the porous support 3. As an example, the retention rate of the separation factor α of the separation membrane 10 when the separation membrane 10 is contacted with nitrogen at a pressure of 2.0 MPa for 5 minutes is 70% or more. Here, the separation factor α is defined as the permeation rate T of nitrogen that permeates the separation membrane 10 when nitrogen at a pressure of 0.6 MPa is supplied to a space adjacent to one side of the separation membrane 10. N2 (GPU) for the carbon dioxide permeation rate T of the separation membrane 10 when carbon dioxide is supplied to the space at a pressure of 0.6 MPa. CO2 (GPU) ratio T CO2 / T N2 means.

[0155] To the best of the inventors' knowledge, no separation membrane has been known to date that has a thickness of 130 μm or less and that has a retention rate of the separation factor α of 70% or more. In another aspect, the present invention provides a separation membrane 10 comprising: a separation functional layer 1; a porous support 3 that supports the separation functional layer 1; and an intermediate layer 2 that is disposed between the separation functional layer 1 and the porous support 3, wherein the thickness of the separation membrane 10 is 130 μm or less, and the retention rate of the separation factor α of the separation membrane 10 is 70% or more when the separation membrane 10 is contacted with nitrogen at a pressure of 2.0 MPa for 5 minutes.

[0156] The retention rate of the separation factor α can be determined in detail by the following method. First, a test piece is prepared by stacking the separation membrane 10 in an initial state on a permeation spacer (#1000 manufactured by KB Seiren Co., Ltd.). In the test piece, the permeation spacer is positioned on the porous support 3 side of the separation membrane 10. The test piece is set in a metal cell and sealed with an O-ring to prevent leakage. Next, nitrogen is injected into the metal cell so that the nitrogen contacts one main surface of the separation membrane 10 (main surface 11 on the separation function layer side). The nitrogen has a temperature of 30°C and a pressure of 0.6 MPa. As a result, a permeated fluid (nitrogen) that has permeated the separation membrane 10 is obtained from the other main surface of the separation membrane 10 (main surface 12 on the porous support side). The flow rate of this permeated fluid is measured with a mass flow meter, and from the obtained results, the nitrogen permeation rate T N2 Identify the GPU.

[0157] Next, carbon dioxide is injected into the metal cell so that the carbon dioxide comes into contact with the main surface 11. The carbon dioxide has a temperature of 30°C and a pressure of 0.6 MPa. As a result, a permeated fluid (carbon dioxide) that has permeated the separation membrane 10 is obtained from the main surface 12. The flow rate of this permeated fluid is measured with a mass flow meter, and from the obtained results, the permeation rate T of carbon dioxide in the initial state is determined. CO2 (GPU) is specified. The transmission rate T in the initial state N2 Transmission rate T for (GPU) CO2 (GPU) ratio T CO2 / T N2 is specified as the initial separation factor α1.

[0158] Next, a pressure test is performed on the separation membrane 10. Specifically, nitrogen is injected into the metal cell so that the nitrogen contacts the main surface 11. In the pressure test, the nitrogen has a temperature of 30°C and a pressure of 2.0 MPa. In the pressure test, the separation membrane 10 is brought into contact with nitrogen at a pressure of 2.0 MPa for 5 minutes. After the pressure test, the separation membrane 10 (test piece) is subjected to the same method as above to measure the permeation rate T N2 (GPU) and transmission rate T CO2 (GPU) is specified. The permeation rate T after the pressure test N2 Transmission rate T for (GPU) CO2 (GPU) ratio T CO2 / T N2 is identified as the separation factor α2 after the pressure test.

[0159] Next, the ratio α2 / α1 of the separation factor α2 after the pressure test to the separation factor α1 in the initial state is calculated. The calculated value obtained can be regarded as the maintenance rate of the separation factor α.

[0160] The retention rate of the separation factor α is preferably 80% or more, and may be 85% or more, 90% or more, 95% or more, or even 98% or more. The upper limit of the retention rate of the separation factor α is, for example, 120% or less, and may be 115% or less, 110% or less, or even 100% or less.

[0161] The initial carbon dioxide permeation rate T CO2 is, for example, 10 GPU or more, and may be 20 GPU or more, 30 GPU or more, 40 GPU or more, 50 GPU or more, 60 GPU or more, or even 70 GPU or more. CO2 The upper limit of the nitrogen permeation rate T is not particularly limited, as the higher the value, the better. For example, it may be 2000 GPU or less. N2 For example, the GPU may be 50 GPUs or less, and may be less than 10 GPUs. -6 ·cm 3 (STP) / (sec cm 2 cm 3 (STP) refers to the volume of carbon dioxide at 1 atmosphere and 0°C.

[0162] The initial separation factor α1 (ratio T CO2 / T N2 ) is, for example, 10 or more, and may be 11 or more, 12 or more, 13 or more, 14 or more, 15 or more, 16 or more, 17 or more, or even 18 or more. The upper limit of the separation factor α1 is, for example, 100 or less, and may be 50 or less.

[0163] Carbon dioxide permeation rate T after pressure test CO2 is, for example, 10 GPU or more, and may be 20 GPU or more, 30 GPU or more, 40 GPU or more, 50 GPU or more, 60 GPU or more, or even 70 GPU or more. CO2 The upper limit of the nitrogen permeation rate T after the pressure test is not particularly limited, but may be, for example, 2000 GPU or less. N2 is, for example, 50 GPUs or less, and may be less than 10 GPUs.

[0164] Separation factor α2 after pressure test (ratio T CO2 / T N2 ) is, for example, 10 or more, and may be 12 or more, 14 or more, 15 or more, 17 or more, or even 20 or more. The upper limit of the separation factor α2 is, for example, 100 or less, and may be 50 or less.

[0165] The separation membrane 10 tends to have a high tensile strength due to the presence of the porous support 3. A separation membrane 10 with a high tensile strength tends to have a high retention rate of the separation factor α. As an example, the tensile strength Y MD is, for example, 5.0 N / 50 mm or more, 10 N / 50 mm or more, 20 N / 50 mm or more, 30 N / 50 mm or more, 50 N / 50 mm or more, 80 N / 50 mm or more, 100 N / 50 mm or more, or even 150 N / 50 mm or more. MD The upper limit is, for example, 500 N / 50 mm or less.

[0166] Furthermore, the tensile strength Y in the CD direction (direction perpendicular to the MD direction) of the separation membrane 10 CDis, for example, 5.0 N / 50 mm or more, and may be 10 N / 50 mm or more, 20 N / 50 mm or more, 30 N / 50 mm or more, or even 50 N / 50 mm or more. CD The upper limit is, for example, 500 N / 50 mm or less.

[0167] Tensile strength Y MD can be measured by the following method. First, the separation membrane 10 is cut to a length of 70 mm in the MD direction and a length of 70 mm in the CD direction to prepare a test specimen. The test specimen is set in a tensile tester so that two chucks are aligned in the MD direction of the test specimen. The maximum stress when a tensile test is performed under the conditions of a chuck distance of 50 mm and a tensile speed of 100 mm / min is defined as the tensile strength Y MD Tensile strength Y CD is the tensile strength Y except that the test specimen is set in the tensile tester so that the two chucks are aligned in the CD direction of the test specimen. MD can be measured by the same method as

[0168] (Applications of Separation Membrane) Applications of the separation membrane 10 of this embodiment include applications for separating acidic gases from mixed gases containing acidic gases. Examples of acidic gases in mixed gases include carbon dioxide, hydrogen sulfide, carbonyl sulfide, sulfur oxides (SOx), hydrogen cyanide, and nitrogen oxides (NOx), with carbon dioxide being preferred. The mixed gas contains other gases in addition to the acidic gas. Examples of other gases include non-polar gases such as hydrogen, nitrogen, and methane, and inert gases such as helium, with nitrogen and methane being preferred. In particular, the separation membrane 10 of this embodiment is suitable for applications for separating carbon dioxide from mixed gases containing carbon dioxide and nitrogen. However, the applications of the separation membrane 10 are not limited to applications for separating acidic gases from the above-mentioned mixed gases.

[0169] <Embodiment of Membrane Separation Apparatus> As shown in Fig. 3, a membrane separation apparatus 100 of this embodiment includes a separation membrane 10 and a tank 20. The tank 20 includes a first chamber 21 and a second chamber 22. The separation membrane 10 is disposed inside the tank 20. Inside the tank 20, the separation membrane 10 separates the first chamber 21 from the second chamber 22. The separation membrane 10 extends from one to the other of a pair of wall surfaces of the tank 20.

[0170] The first chamber 21 has an inlet 21 a and an outlet 21 b. The second chamber 22 has an outlet 22 a. The inlet 21 a, the outlet 21 b, and the outlet 22 a are preferably openings formed in the wall surface of the tank 20.

[0171] Membrane separation using the membrane separation device 100 is performed by the following method. First, a gas mixture 30 containing an acidic gas is supplied to the first chamber 21 through the inlet 21a. The concentration of the acidic gas in the gas mixture 30 is not particularly limited, and is, for example, 0.01 vol% (100 ppm) or more under standard conditions, preferably 1 vol% or more, more preferably 10 vol% or more, even more preferably 30 vol% or more, and particularly preferably 50 vol% or more. The upper limit of the concentration of the acidic gas in the gas mixture 30 is not particularly limited, and is, for example, 90 vol% under standard conditions.

[0172] The pressure inside the first chamber 21 may be increased by the supply of the mixed gas 30. The membrane separation apparatus 100 may further include a pump (not shown) for increasing the pressure of the mixed gas 30. The pressure of the mixed gas 30 supplied to the first chamber 21 is, for example, 0.1 MPa or more, preferably 0.3 MPa or more.

[0173] The second chamber 22 may be depressurized while the gas mixture 30 is supplied to the first chamber 21. The membrane separation apparatus 100 may further include a pump (not shown) for depressurizing the second chamber 22. The second chamber 22 may be depressurized so that the space within the second chamber 22 is reduced in pressure by, for example, 10 kPa or more, preferably 50 kPa or more, and more preferably 100 kPa or more relative to the atmospheric pressure in the measurement environment.

[0174] By supplying the gas mixture 30 into the first chamber 21, a permeated fluid 35 having a higher acid gas content than the gas mixture 30 can be obtained on the other side of the separation membrane 10. That is, the permeated fluid 35 is supplied to the second chamber 22. The permeated fluid 35 preferably contains an acid gas as a main component. However, the permeated fluid 35 may contain small amounts of gases other than the acid gas. The permeated fluid 35 is discharged to the outside of the tank 20 through the outlet 22a.

[0175] The concentration of the acid gas in the mixed gas 30 gradually decreases from the inlet 21a to the outlet 21b of the first chamber 21. The mixed gas 30 (non-permeated fluid 36) treated in the first chamber 21 is discharged to the outside of the tank 20 through the outlet 21b.

[0176] The membrane separation apparatus 100 of this embodiment is suitable for a continuous membrane separation method, but may also be used for a batch-type membrane separation method.

[0177] <Modifications of Membrane Separation Device> The membrane separation device 100 may be a spiral membrane element, a hollow fiber membrane element, or the like. Fig. 4 shows a spiral membrane element. The membrane separation device 110 in Fig. 4 includes a central tube 41 and a stack 42. The stack 42 includes the separation membrane 10.

[0178] The central tube 41 has a cylindrical shape. A plurality of holes are formed on the surface of the central tube 41 to allow the permeating fluid 35 to flow into the interior of the central tube 41. Examples of materials for the central tube 41 include resins such as acrylonitrile-butadiene-styrene copolymer resin (ABS resin), polyphenylene ether resin (PPE resin), and polysulfone resin (PSF resin); and metals such as stainless steel and titanium. The inner diameter of the central tube 41 is, for example, in the range of 20 to 100 mm.

[0179] The laminate 42 further includes a feed-side channel material 43 and a permeate-side channel material 44 in addition to the separation membrane 10. The laminate 42 is wound around a central tube 41. The membrane separation device 110 may further include an exterior material (not shown).

[0180] The feed-side channel material 43 and the permeate-side channel material 44 may be, for example, a resin net made of polyphenylene sulfide (PPS) or ethylene-chlorotrifluoroethylene copolymer (ECTFE).

[0181] Membrane separation using the membrane separation device 110 is performed in the following manner. First, the gas mixture 30 is supplied to one end of the wound stack 42. The permeated fluid 35 that has permeated the separation membrane 10 of the stack 42 moves into the interior of the central tube 41. The permeated fluid 35 is discharged to the outside through the central tube 41. The gas mixture 30 (non-permeated fluid 36) that has been treated in the membrane separation device 110 is discharged to the outside from the other end of the wound stack 42. This allows acidic gases to be separated from the gas mixture 30.

[0182] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto.

[0183] (Example 1) [Synthesis of Polyimide] First, polyimide was synthesized using an automatic polymerization apparatus (Mettler Toledo, EasyMax402). A separable flask (volume 400 mL) attached to the apparatus was equipped with a Dimroth tube, a stirring rod, an internal thermometer, a nitrogen inlet tube, and a flat stopper. A cooling liquid set to 10°C was circulated through the Dimroth chiller. N2 gas was circulated through the flask at a flow rate of 100 mL / min. The stirring speed was set to 300 rpm. Next, 96.1 g of 1-methyl-2-pyrrolidone (super-dehydrated) as a solvent and 2.62 g (17.5 mmol) of 2,4,6-trimethyl-1,3-phenylenediamine (TrMPD) as diamines, 4.80 g (17.5 mmol) of 3,7-diamino-2,8-dimethyldibenzothiophenesulfone (DDBT), and 2.11 g (0.5 mmol) of 5,5'-methylenebis(2-aminobenzoic acid) (MBAA) were added to the flask. The diamine was dissolved in the solvent by stirring at room temperature. To the resulting solution, 9.53 g (35.5 mmol) of naphthalene-1,4,5,8-tetracarboxylic dianhydride (NTDA) as a tetracarboxylic dianhydride and 8.54 g (70 mmol) of benzoic acid were further added. The jacket temperature of the apparatus was raised to 180°C, and the mixture was stirred for 8 hours. At this time, the internal temperature of the flask was 172 to 175° C. After stirring, the internal temperature of the flask was cooled to 25° C. and allowed to stand overnight.

[0184] Next, 9.04 g (70 mmol) of isoquinoline was added, and the jacket temperature was raised again to 180°C, followed by stirring for 8 hours. After leaving the reaction solution to stand overnight, 226 g of 1-methyl-2-pyrrolidone was added to dilute the reaction solution. Next, using a dropping funnel, 650 mL of methanol was added dropwise to the reaction solution over approximately 30 minutes, and reprecipitation purification was carried out. The precipitated polyimide was filtered off, and the polyimide was washed twice with 300 mL of methanol. After washing, the filtered polyimide was dried in a hot air circulation dryer at 60°C for 15 hours, and then further dried in a vacuum dryer at 100°C for 8 hours. This yielded 17.1 g of polyimide.

[0185] [Preparation of Separation Functional Layer] Next, polyimide was added to a 50 mL screw tube, and N-methyl-2-pyrrolidone (NMP) as a solvent and acetylacetone as a ligand were added to obtain a mixed solution. This mixed solution was stirred for 5 minutes and degassed twice. Next, NMP and Al(acac)3 as a metal complex were added to another screw tube, and the mixture was subjected to ultrasonic treatment using an ultrasonic cleaner to obtain an Al(acac)3 solution. The Al(acac)3 solution and the mixed solution were further mixed, and the mixture was stirred for 5 minutes and degassed twice to obtain a coating solution containing polyimide. The stirring and degassing were performed using a Thinky Mixer. The polyimide content in the coating solution was 8 wt%.

[0186] Next, the above coating solution was applied onto a release-treated polyimide film (manufactured by Fujiko Co., Ltd., SCA0) to prepare a coating film (thickness: 30 μm). This coating film was dried at 130°C for 10 minutes to obtain a separation functional layer with a thickness of 2 μm. Note that, as the coating film dried, the dissociative proton of the functional group g (carboxyl group) contained in the polyimide was exchanged with Al of the metal complex. This resulted in the formation of an Al salt of the functional group g.

[0187] Next, a silicone-based adhesive (KR-3701, manufactured by Shin-Etsu Silicones Co., Ltd.) was diluted with toluene to prepare a coating solution with a solids concentration of 6 wt%. This coating solution was applied onto the separation functional layer to prepare a coating film (thickness 100 μm). This coating film was dried at 130°C for 3 minutes to form an intermediate layer with a thickness of 3 μm. This resulted in a laminate having a polyimide film, a separation functional layer, and an intermediate layer in this order.

[0188] Next, the intermediate layer of the above laminate was superimposed on a porous support, and they were pressure-bonded under conditions of 0.3 MPa and 1 m / min. As the porous support, a PET nonwoven fabric (N401, manufactured by Awa Paper Co., Ltd.) was used. Next, double-sided tape was attached to the surface of the polyimide film and fixed to the support. Furthermore, tape was attached to the surface of the porous support, and the laminate of the separation function layer, intermediate layer, and porous support was slowly peeled off from the polyimide film by grasping the tape. This gave the separation membrane of Example 1.

[0189] Examples 2 to 5 Separation membranes of Examples 2 to 5 were obtained in the same manner as in Example 1, except that the type of porous support and the thickness of each layer were changed as shown in Table 1.

[0190] (Example 6) First, a separation functional layer having a thickness of 4 μm was formed on a polyimide film by the same method as in Example 1. This separation functional layer was peeled off from the polyimide film to obtain a separation membrane of Example 6 consisting only of the separation functional layer.

[0191] [Physical properties of porous support] (ISO air permeability) The ISO air permeability of the porous support used to prepare the separation membrane was measured in accordance with the Oken type testing machine method specified in JIS P8117: 2009. The ISO air permeability was measured using a digital Oken type air permeability tester EGO1 (manufactured by Asahi Seiko Co., Ltd.) under conditions of a measurement pressure of 0.05 MPa and a measurement time of 60 seconds.

[0192] (Area Load Ratio Smr(c1)) For the porous support used in producing the separation membrane, the surface on the intermediate layer side was observed with a laser microscope by the method described above, and a three-dimensional analysis was performed to create a load curve. As the laser microscope, a hybrid laser microscope OPTELICS manufactured by Lasertec was used, and as the objective lens, an M-PLAN APO 50X manufactured by Mitutoyo Corporation was used. Using the obtained load curve, a height c1 was identified whose difference from the height c0 when the area load ratio was 0% coincided with the thickness of the intermediate layer, and the area load ratio Smr(c1) corresponding to the height c1 was identified.

[0193] [Peel Strength] A layer having the same composition and thickness as the intermediate layer of the separation membrane was formed on the evaluation sheet, and the peel strength between the intermediate layer and the porous support was measured by the method described above.

[0194] [Physical Properties of Separation Membrane] (Tensile Strength) The tensile strength Y in the MD direction of the produced separation membrane was measured by the above-mentioned method. MD and the tensile strength Y in the CD direction CD The tensile tester used was an Autograph AGX-V manufactured by Shimadzu Corporation.

[0195] (Retention rate of separation factor α) For the prepared separation membrane, the nitrogen permeation rate T N2 (GPU) and carbon dioxide permeation rate T CO2 (GPU) and measure the ratio T CO2 / T N2 was specified as the initial separation factor α1. Furthermore, a pressure test was carried out by the above-mentioned method, and the nitrogen permeation rate T N2 (GPU) and carbon dioxide permeation rate T CO2 (GPU) and measure the ratio T CO2 / T N2 was specified as the separation factor α2 after the pressure test. The ratio α2 / α1 of the separation factor α2 after the pressure test to the separation factor α1 in the initial state was calculated, and the calculated value was regarded as the maintenance rate of the separation factor α.

[0196]

[0197]

[0198] The abbreviations in Table 1 are as follows: N401: PET nonwoven fabric (N401, manufactured by Awa Paper Co., Ltd.) S54: PET nonwoven fabric (S54, manufactured by Hokuetsu Corporation) N301: PET nonwoven fabric (N301, manufactured by Awa Paper Co., Ltd.) PS0100S-thin: PPS nonwoven fabric (PS0100S-thin, manufactured by Hirose Paper Co., Ltd.)

[0199] As can be seen from Tables 1 and 2, the thickness of the separation membrane could be adjusted to be small in Examples 1 to 5, in which the areal load ratio Smr(c1) of the surface of the porous support facing the intermediate layer was less than 80%. The separation membranes of Examples 1 to 5 can be easily increased in membrane area that can be installed in a membrane separation device (especially a spiral membrane element), and therefore can be said to be suitable for membrane separation devices.

[0200] Furthermore, the separation membranes of Examples 1 to 5 had a higher retention rate of the separation factor α and better pressure resistance than the separation membrane of Example 6, which was not provided with a porous support.

[0201] The separation membranes of Examples 1 to 5 had a carbon dioxide permeation rate T CO2 The separation coefficient α1 was 10 or more, both of which were sufficient for practical use.

[0202] The separation membrane of this embodiment is suitable for separating an acid gas from a gas mixture containing the acid gas, and in particular, for separating carbon dioxide from off-gas of a chemical plant or thermal power plant.

Claims

1. A separation membrane comprising: a separation functional layer; a porous support supporting the separation functional layer; and an intermediate layer disposed between the separation functional layer and the porous support, the porous support having a surface S1 facing the intermediate layer, the surface S1 having an areal load ratio Smr(c1) of less than 80% as determined by the following test. Test: A three-dimensional analysis is performed on the surface S1 of the porous support to obtain a load curve as defined in Japanese Industrial Standards (JIS) B0681-2:2018. In the load curve, a height c1 is identified whose difference from the height c0 when the areal load ratio is 0% and which coincides with the thickness of the intermediate layer. The areal load ratio corresponding to the height c1 is read and identified as the areal load ratio Smr(c1).

2. The separation membrane according to claim 1, wherein the areal loading ratio Smr(c1) is 0.04% or more.

3. The separation membrane according to claim 1, having a thickness of 130 μm or less.

4. A separation membrane comprising a separation functional layer, a porous support supporting the separation functional layer, and an intermediate layer disposed between the separation functional layer and the porous support, the thickness of the separation membrane being 130 μm or less, and the retention rate of the separation factor α of the separation membrane being 70% or more when the separation membrane is contacted with nitrogen at a pressure of 2.0 MPa for 5 minutes, wherein the separation factor α is the permeation rate T of nitrogen that permeates the separation membrane when nitrogen at a pressure of 0.6 MPa is supplied to a space adjacent to one side of the separation membrane. N2 (GPU) is the permeation rate T of carbon dioxide that permeates the separation membrane when carbon dioxide at a pressure of 0.6 MPa is supplied to the space. CO2 (GPU) ratio T CO2 / T N2 means...

5. The separation membrane according to claim 1 or 4, wherein the porous support is a fibrous structure.

6. The separation membrane according to claim 1 or 4, wherein the thickness of the porous support is 125 μm or less.

7. The ISO air permeability of the porous support is 10.0 x 10 4 The separation membrane according to claim 1 or 4, having a viscosity of 1 μm / (Pa·s) or more.

8. The separation membrane according to claim 1 or 4, wherein the separation functional layer comprises polyimide.

9. The separation membrane according to claim 8, wherein the polyimide contains a structural unit derived from a tetracarboxylic dianhydride having a six-membered ring acid anhydride structure.

10. The separation membrane according to claim 9, wherein the structural unit is represented by the following formula (A1): In the formula (A1), R 1a ~R 4a are each independently a hydrogen atom or any substituent.

11. The separation membrane according to claim 1 or 4, wherein the separation functional layer has a thickness of 5.0 μm or less.

12. The separation membrane according to claim 1 or 4, wherein the intermediate layer is formed from a pressure-sensitive adhesive composition.

13. The separation membrane of claim 12, wherein the adhesive composition comprises a silicone-based polymer.

14. The separation membrane according to claim 1 or 4, wherein the thickness of the intermediate layer is 5.0 μm or less.

15. The separation membrane according to claim 1 or 4, wherein the peel strength between the intermediate layer and the porous support is 0.25 N / 25 mm or more.

Citation Information

Patent Citations

  • Sulfonated aromatic polyimide and electrolyte film composed of the same

    JP2006265496A

  • Separation film

    WO2021192745A1

  • Separation membrane and method for manufacturing same

    WO2022190612A1

  • Spiral membrane element and membrane separation system

    WO2022190938A1

  • Manufacturing method for separation film and separation film

    WO2022196306A1