Elastomer composition, method for producing elastomer composition, sealing material, and method for producing sealing material
The combination of a crosslinkable fluoroelastomer and a perfluoro skeleton compound with specific viscosity characteristics addresses the mixing challenges of conventional compositions, resulting in a sealing material with enhanced plasma resistance and balanced properties for semiconductor applications without silica.
Patent Information
- Application Number
- PCT/JP2024/004774
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-02-13
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional uncrosslinked rubber compositions, such as those containing crosslinkable fluoroelastomers and liquid or oily perfluoro skeleton compounds, face difficulties in achieving uniform mixing and limited usage amounts, leading to challenges in forming sealing materials with desired physical properties, especially in applications like semiconductor manufacturing where plasma resistance is crucial.
A composition comprising a crosslinkable fluoroelastomer and a compound with a perfluoro skeleton, synthesized to have a viscosity of 1000 to 9000 Pa·s, is used, allowing for a uniform mixture with a higher content of the perfluoro skeleton compound, which enhances plasma resistance and simplifies the formation of a well-balanced sealing material without the need for silica fillers.
The resulting elastomer composition exhibits excellent plasma resistance, hardness, tensile strength, elongation at break, and 100% Mo properties, making it suitable for applications in plasma processing equipment without the use of silica, and can be easily formed into a uniform and effective sealing material.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Elastomer composition, method for producing elastomer composition, sealant, and method for producing sealant
[0001] One embodiment of the present invention relates to an elastomer composition, a method for producing an elastomer composition, a seal material, or a method for producing a seal material.
[0002] BACKGROUND ART Sealing materials have been used in a wide variety of applications. Among these applications, sealing materials used in semiconductor manufacturing equipment and the like are an example of an application that places the greatest load on sealing materials.
[0003] Crosslinkable fluoroelastomers such as fluoroelastomers (FKM) and perfluoroelastomers (FFKM) are used as such sealing materials because they can provide sealing materials with excellent plasma resistance (radical resistance). For example, Patent Document 1 discloses an uncrosslinked rubber composition used for producing sealing materials, which contains a hydrogen-containing fluororubber that is a crosslinkable fluoroelastomer and a liquid hydrogen site protecting agent.
[0004] Japanese Patent Application Laid-Open No. 2019-52226
[0005] In conventional uncrosslinked rubber compositions such as the composition described in Patent Document 1, liquid or oily perfluoro-skeleton compounds (hydrogen site protectors in Patent Document 1) have been used to obtain sealing materials with excellent plasma resistance (radical resistance). To form a molded product such as a sealing material exhibiting desired physical properties from such an uncrosslinked rubber composition, it is necessary for the components in the composition to be uniformly mixed. However, it has been found that crosslinkable fluoroelastomers and liquid or oily perfluoro-skeleton compounds are difficult to mix, which limits the amount of liquid or oily perfluoro-skeleton compounds that can be used with crosslinkable fluoroelastomers, and it is not easy to prepare a uniform composition of crosslinkable fluoroelastomers and liquid or oily perfluoro-skeleton compounds.
[0006] One embodiment of the present invention provides an elastomer composition that is easy to prepare into a uniform composition and that contains a crosslinkable fluoroelastomer and a compound having a perfluoro skeleton.
[0007] An example of the configuration of the present invention is as follows.
[0008] [1] An elastomer composition comprising: a crosslinkable fluoroelastomer (A); and a compound (B) having a perfluoro skeleton, the viscosity of which at 23°C is measured using a cone-plate viscometer in accordance with JIS Z 8803:2011, in accordance with the method for measuring viscosity of liquids, of 1000 to 9000 Pa s.
[0009] [2] The elastomer composition according to [1], wherein the content of the compound (B) having a perfluoro skeleton is 5 parts by mass or more per 100 parts by mass of the crosslinkable fluoroelastomer (A).
[0010] [3] The elastomer composition according to [1] or [2], wherein the compound (B) having a perfluoro skeleton is a reaction product of a compound having a perfluoro skeleton with an ethylenically unsaturated bond and a reactive organosilicon compound having a hydrosilyl group.
[0011] [4] A method for producing an elastomer composition, comprising the following steps 1 and 2: Step 1: reacting a compound having a perfluoro skeleton containing an ethylenically unsaturated bond with a reactive organosilicon compound having a hydrosilyl group to synthesize a compound (B) having a perfluoro skeleton with a viscosity of 1,000 to 9,000 Pa s at 23°C, as measured using a cone-plate viscometer in accordance with JIS Z 8803:2011, a method for measuring the viscosity of liquids; and Step 2: mixing the crosslinkable fluoroelastomer (A) with the compound (B) having a perfluoro skeleton obtained in Step 1.
[0012] [5] In the step 2, the compound (B) having a perfluoro skeleton is used in an amount of 5 parts by mass or more relative to 100 parts by mass of the crosslinkable fluoroelastomer (A). [6] The method for producing an elastomer composition according to [4].
[0013] [6] A sealing material obtained from the elastomer composition according to any one of [1] to [3].
[0014] [7] A method for producing a sealing material, comprising a step of crosslinking the elastomer composition according to any one of [1] to [3].
[0015] According to one embodiment of the present invention, an elastomer composition containing a crosslinkable fluoroelastomer and a compound having a perfluoro skeleton can be easily prepared into a uniform composition in a short time. Furthermore, according to one embodiment of the present invention, even elastomer compositions containing a high proportion of the compound having a perfluoro skeleton (elastomer compositions using a compound having a perfluoro skeleton in an amount that would not be able to be uniform when a liquid or oily perfluoro skeleton compound is used) can be easily prepared into a uniform composition, thereby easily obtaining elastomer compositions and sealing materials that are particularly excellent in plasma resistance (radical resistance). While the use of millable-type perfluoro skeleton compounds requires silica (an inorganic filler), according to one embodiment of the present invention, desired elastomer compositions and sealing materials can be easily obtained without the use of silica, which can generate particles in plasma atmospheres, etc. Furthermore, according to one embodiment of the present invention, a sealing material can be obtained that is well-balanced in terms of hardness, tensile strength, elongation at break, and tensile stress at 100% elongation (100% Mo), making it suitable for use in semiconductor manufacturing equipment and plasma processing equipment.
[0016] FIG. 1 is an explanatory diagram relating to the test of adhesive strength in the following examples.
[0017] <Elastomer Composition> An elastomer composition according to one embodiment of the present invention (hereinafter also referred to as "the composition") contains a crosslinkable fluoroelastomer (A) and a compound (B) having a perfluoro skeleton, which has a viscosity of 1000 to 9000 Pa s at 23°C, measured using a cone-plate viscometer in accordance with JIS Z 8803:2011, a method for measuring viscosity of liquids.
[0018] <Crosslinkable fluoroelastomer (A)> The crosslinkable fluoroelastomer (A) is not particularly limited, and conventionally known crosslinkable fluoroelastomers can be used. The elastomer (A) used in the present composition may be one type or two or more types. In the present invention, "elastomer" and "rubber" have the same meaning, and there is no particular distinction between them.
[0019] The elastomer (A) is also called unvulcanized fluororubber, and examples of crosslinked types include peroxide crosslinking, polyol crosslinking, amine crosslinking, radiation crosslinking, etc. Among these, peroxide-crosslinkable fluoroelastomers are preferred, since they do not require the use of an acid acceptor that can be a source of particle generation in a plasma atmosphere, etc., and there is no risk of particle generation during use of the resulting sealing material.
[0020] Specific examples of the elastomer (A) include fluoroelastomers (FKM), perfluoroelastomers (FFKM), tetrafluoroethylene-propylene elastomers (FEPM), and fluorine-containing thermoplastic elastomers (e.g., elastomers containing at least one type of elastomeric polymer chain segment and at least one type of non-elastomeric polymer chain segment, at least one of which is a fluorine-containing polymer chain segment).
[0021] The elastomer (A) may be synthesized by a conventionally known method or may be a commercially available product, such as "Dai-el" manufactured by Daikin Industries, Ltd., "Viton" manufactured by Chemours, "Dyneon" manufactured by 3M, or "Technoflon" manufactured by Solvay.
[0022] The elastomer (A) is preferably an elastomer capable of producing a sealing material resistant to plasma (plasma etching treatment) used in various semiconductor dry processes, and more preferably FKM, which has relatively good plasma resistance and excellent sealing properties. FKM is also preferred because it is inexpensive and versatile.
[0023] There are no particular limitations on the FKM, but examples include polymers containing hydrogen atoms (carbon-hydrogen bonds) in the polymer main chain, and specifically, it is preferable that the FKM contains structural units derived from vinylidene fluoride.
[0024] The FKM is not particularly limited, but specific examples include vinylidene fluoride-hexafluoropropylene polymers, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene polymers, tetrafluoroethylene-propylene polymers, vinylidene fluoride-propylene-tetrafluoroethylene polymers, ethylene-tetrafluoroethylene-perfluoroalkyl vinyl ether polymers, vinylidene fluoride-tetrafluoroethylene-perfluoroalkyl vinyl ether polymers, and vinylidene fluoride-perfluoroalkyl vinyl ether polymers. A suitable example of the perfluoroalkyl vinyl ether is perfluoromethyl vinyl ether.
[0025] Among these, ternary polymers are preferred because of their excellent plasma resistance, heat resistance, chemical resistance, etc., and vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene polymers are more preferred.
[0026] The peroxide-crosslinkable fluoroelastomer preferably has a functional group such as an iodine group, a bromine group, a cyano group, a peroxy group, or an unsaturated group, and from the viewpoint of ease of introduction of the functional group, an iodine group or a bromine group is more preferred. The fluoroelastomer having an iodine group and / or a bromine group can be obtained, for example, by using one or more saturated or unsaturated iodine- and / or bromine-containing compounds when synthesizing the elastomer.
[0027] Examples of the iodine- and / or bromine-containing compound include compounds represented by the following formula (I) or (II): By using the compound represented by the following formula (I), a fluoroelastomer having an iodine group and / or a bromine group in the side chain can be synthesized, and by using the compound represented by the following formula (II), a fluoroelastomer having an iodine group and / or a bromine group at the end can be synthesized.
[0028] CY 1 2 = CY 2 RfX (I) [Y 1 and Y 2 are each independently a fluorine atom, a hydrogen atom or a methyl group, Rf is a linear or branched fluorine-containing alkylene group in which some or all of the hydrogen atoms have been substituted with fluorine atoms, or a group containing an ether bond in part of the fluorine-containing alkylene group, and X is an iodine atom or a bromine atom.
[0029] Specific examples of the compound represented by formula (I) include compounds described in WO 2009 / 119409.
[0030] I n Br m R (II) [R is a fluorohydrocarbon group having 1 to 12 carbon atoms, n and m each independently represent an integer of 0 to 2, and n+m is 1 or 2.]
[0031] Specific examples of the compound represented by formula (II) include compounds described in JP-A Nos. 2002-97329 and 2008-56739.
[0032] The fluorine content of the elastomer (A) is not particularly limited, but from the viewpoint of easily obtaining a desired sealing material, it is preferably 55% by mass or more, more preferably 60% by mass or more, even more preferably 63% by mass or more, particularly preferably 65% by mass or more, and more preferably 73% by mass or less, even more preferably 71% by mass or less. 19 F-NMR and 1 It can be measured or calculated by elemental analysis of fluorine using H-NMR or mass spectrometry (MS spectrometry), etc. The fluorine content in the present invention is a value rounded off to the nearest whole number.
[0033] The elastomer (A) preferably comprises a crosslinkable fluoroelastomer (A1) having a fluorine content of 69% by mass or more and a crosslinkable fluoroelastomer (A2) having a fluorine content of 55 to 68% by mass. By using at least two crosslinkable fluoroelastomers having fluorine contents within the above ranges, a uniform elastomer composition can be easily obtained in a short time, an elastomer composition with excellent moldability can be easily obtained, and a sealing material with a good balance of hardness, tensile strength, elongation at break, and 100% Mo can be easily obtained.
[0034] The fluorine content of the elastomer (A1) is preferably 70% by mass or more, and preferably 73% by mass or less, more preferably 71% by mass or less. The fluorine content of the elastomer (A2) is preferably 60 to 68% by mass, more preferably 63 to 68% by mass, and even more preferably 65 to 68% by mass.
[0035] The Mooney viscosity of the elastomer (A) is preferably 10 or more, more preferably 15 or more, even more preferably 18 or more, and preferably 140 or less, more preferably 120 or less, still more preferably 80 or less, and particularly preferably 60 or less. When the Mooney viscosity of the elastomer (A) is within the above range, an elastomer composition having excellent moldability, particularly extrusion property, can be easily obtained. In this specification, the Mooney viscosity refers to the Mooney viscosity (ML1+10) at 121°C measured in accordance with ASTM D 1646.
[0036] The content of the elastomer (A) in the solid content of the composition is preferably 40% by mass or more, more preferably 50% by mass or more, and preferably 95% by mass or less, more preferably 93% by mass or less. When the content of the elastomer (A) is within the above range, a sealing material can be easily obtained that has excellent chemical resistance such as plasma resistance and chemical resistance, and a well-balanced excellent hardness, tensile strength, elongation at break, and 100% Mo. In this specification, the solid content refers to components other than the solvent.
[0037] When the composition contains the elastomer (A1), the content of the elastomer (A1) in the solid content of the composition is preferably 40% by mass or more, more preferably 50% by mass or more, and is preferably 95% by mass or less, more preferably 85% by mass or less. When the content of the elastomer (A1) is within the above range, a sealing material having excellent chemical resistance such as plasma resistance and chemical resistance can be easily obtained.
[0038] When the composition contains the elastomer (A2), the content of the elastomer (A2) in the solid content of the composition is preferably 2% by mass or more, more preferably 5% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less. When the content of the elastomer (A2) is within the above range, a sealing material having a good balance of moldability and chemical resistance can be easily obtained.
[0039] When the composition contains elastomers (A1) and (A2), the content of the elastomer (A1) relative to the total content of the elastomers (A1) and (A2) in the composition is preferably 60% by mass or more, more preferably 65% by mass or more, and preferably 95% by mass or less. When the mass ratio of the contents of the elastomers (A1) and (A2) is within the above range, a uniform elastomer composition can be easily obtained in a short time, an elastomer composition with excellent moldability can be easily obtained, and a sealing material with a well-balanced excellent hardness, tensile strength, elongation at break, and 100% Mo can be easily obtained.
[0040] <Compound (B) Having a Perfluoro Skeleton> The compound (B) having a perfluoro skeleton is not particularly limited, as long as it has a viscosity of 1000 to 9000 Pa·s at 23°C, as measured using a cone-plate viscometer in accordance with JIS Z 8803:2011, a method for measuring the viscosity of liquids, and has a perfluoro skeleton. The use of compound (B) makes it easy to obtain a sealing material with excellent plasma resistance (radical resistance). Furthermore, the use of compound (B) makes it easy to obtain a sealing material with a well-balanced excellent hardness, tensile strength, elongation at break, and 100% Mo. The compound (B) used in the present composition may be one type or two or more types. The phrase "the composition contains compound (B)" refers to the use of compound (B) as a raw material in preparing the present composition. The phrase "the composition contains two or more types of compound (B)" refers to the use of two or more types of compound (B) as raw materials in preparing the present composition.
[0041] The viscosity of compound (B) at 23°C, measured using a cone-and-plate viscometer in accordance with JIS Z 8803:2011, is 1,000 to 9,000 Pa·s, preferably 3,000 to 8,000 Pa·s. Compound (B) having a viscosity within this range is a gel-like or slime-like compound, different from liquid, oil-like, or millable-type compounds. The viscosity of compound (B) refers to the viscosity before mixing with elastomer (A) and the other components described below, i.e., the viscosity of the compound as a raw material when preparing the composition, within the above range.
[0042] The minimum torque (ML) of compound (B) at 60°C measured with a curastometer is preferably less than 0.5 kgf cm. Note that this minimum torque (ML) also refers to the minimum torque (ML) of the raw material before being mixed with elastomer (A) and the other components described below. Specifically, the minimum torque (ML) is a value measured under the following conditions using a Curastometer TYPER (for rubber) manufactured by JSR Trading Co., Ltd. Sample: 10 g Temperature: 60°C Amplitude angle: ±3° Measurement time: 10 minutes
[0043] The content of compound (B) in the present composition is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and preferably 100 parts by mass or less, more preferably 50 parts by mass or less, relative to 100 parts by mass of elastomer (A), from the viewpoints that an elastomer composition having excellent roll processability can be easily obtained, and a sealing material having excellent plasma resistance (radical resistance) can be easily obtained, etc. According to one embodiment of the present invention, a uniform elastomer composition can be obtained even when compound (B) is used in an amount that would not allow a uniform composition to be obtained when a liquid or oily perfluoroskeleton compound is used, and therefore a sealing material having even more excellent plasma resistance (radical resistance) can be easily obtained, and the content of compound (B) in the present composition is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and preferably 100 parts by mass or less, relative to 100 parts by mass of elastomer (A).
[0044] When the present composition contains the compound (B) and the crosslinking agent (C) described below, from the viewpoint that a sealing material having more excellent plasma resistance can be easily obtained, etc., the mass ratio of the content of the compound (B) to the content of the crosslinking agent (C) in the present composition (content of the compound (B) / content of the crosslinking agent (C)) is preferably 0.5 or more, more preferably 1 or more, and is preferably 80 or less, more preferably 60 or less.
[0045] Compound (B) can be obtained by reacting compound (b1) having a perfluoro skeleton and an ethylenically unsaturated bond with reactive organosilicon compound (b2) having a hydrosilyl group. Note that when a sealing material (molded article) is formed from a composition containing elastomer (A), compound (b1), and compound (b2) as follows, for example, the elastomer (A) reacts with compound (b1) and / or compound (b2), and therefore the resulting composition does not contain elastomer (A) and compound (B).
[0046] The viscosity of each of compound (b1) and compound (b2) at 23°C, measured using a cone-plate viscometer in accordance with the method for measuring viscosity of liquids specified in JIS Z 8803:2011, is preferably 1 to 30 Pa s, and more preferably 2 to 10 Pa s.
[0047] As the compound (b1) and the compound (b2), commercially available products such as "SIFEL" (manufactured by Shin-Etsu Chemical Co., Ltd.) may be used. Note that, as commercially available products of the compound (B), there are one-component products and two-component products, and either of these may be used.
[0048] The amount of compound (b1) used in the reaction is preferably 1 to 80% by mass, more preferably 40 to 60% by mass, based on 100% by mass of the total of compound (b1) and compound (b2).
[0049] The reaction conditions are not particularly limited as long as a compound (B) having a perfluoro skeleton within the above-mentioned viscosity range can be synthesized. The reaction temperature is preferably 100 to 250°C, more preferably 120 to 220°C, and the reaction time is preferably 20 minutes to 3 hours, more preferably 30 minutes to 2 hours. When compounds within the above-mentioned viscosity range are used as the raw materials for the reaction, compound (b1) and compound (b2), a portion of the reaction product obtained by the reaction under the above-mentioned reaction conditions is extracted and the viscosity is measured. If the viscosity is within the range of 1000 to 9000 Pa s, the reaction is stopped. If the viscosity is below 1000 Pa s, the reaction temperature can be changed as necessary and the reaction can be continued to obtain a compound (B) having a viscosity within the range of 1000 to 9000 Pa s. In addition, during the reaction, an additive such as a catalyst (e.g., the catalysts described in JP-A-2003-183402, JP-A-11-116684, etc.) may be used.
[0050] <Compound (b1)> The compound (b1) is a compound having a perfluoro skeleton with an ethylenically unsaturated bond, specifically, a compound having a perfluoro skeleton with an ethylenically unsaturated bond-containing group, and is a compound other than the elastomer (A). One type of compound (b1) may be used, or two or more types may be used.
[0051] Examples of the ethylenically unsaturated bond-containing group include alkenyl groups having 2 to 8 carbon atoms, such as vinyl, methylvinyl, allyl, propenyl, isopropenyl, butenyl, pentenyl, hexenyl, and heptenyl, as well as vinylphenyl, (meth)acryloyl, allyloxy, styryl, and propargyl groups. Among these, alkenyl groups are preferred, alkenyl groups having 2 to 4 carbon atoms are more preferred, and vinyl groups are particularly preferred. Compound (b) may have two or more types of ethylenically unsaturated bonds.
[0052] Examples of the compound (b1) include a compound having a perfluoropolyether structure with an ethylenically unsaturated bond and a compound having a perfluoroalkylene structure with an ethylenically unsaturated bond. Among these, a compound having a perfluoropolyether structure with an ethylenically unsaturated bond (hereinafter also referred to as "compound (b1-1)") is preferred.
[0053] Compound (b1-1) The compound (b1-1) is preferably a perfluoropolyether having two or more ethylenically unsaturated bonds in one molecule.
[0054] Suitable examples of the compound (b1-1) include the compounds described in JP-A-2003-183402, JP-A-11-116684, JP-A-11-116685, and JP-A-2015-67737.
[0055] An example of the compound (b1-1) is a compound represented by the following formula (1): 1 -(X) p -(Rf-Q) a -Rf-(X) p -Z 2 ...(1)
[0056] X independently represents -CH2-, -CH2O-, -CH2OCH2-, *-Si(R 2 )2-Ph-(Ph: phenylene group), *-Y-NR 1 -SO2- or *-Y-NR 1 -CO- (wherein Y is -CH2- or *-Si(R 2)2-Ph-. In addition, the * portion is Z 1 or Z 2 Rf is independently a divalent perfluoropolyether group (divalent perfluorooxyalkylene group). p is independently 0 or 1. a is an integer of 0 or more, preferably an integer of 0 to 10, more preferably an integer of 0 to 6. Q is independently a group represented by the following formula (2), (3), or (4):
[0057] R 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms, particularly 1 to 8 carbon atoms, and examples thereof include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, t-butyl, pentyl, hexyl, octyl, and decyl groups; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl groups; alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, and hexenyl groups; aryl groups such as phenyl, tolyl, xylyl, and naphthyl groups; aralkyl groups such as benzyl, phenylethyl, and phenylpropyl groups; and groups in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms or the like (e.g., fluorine-substituted alkyl groups such as chloromethyl, chloropropyl, bromoethyl, 3,3,3-trifluoropropyl, and 3,3,4,4,5,5,6,6,6-nonafluorohexyl groups).
[0058] R 1 is a hydrogen atom or the R 2 is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms, particularly 1 to 8 carbon atoms, similar to the groups exemplified as R 2 Examples include alkyl groups such as a methyl group, an ethyl group, a propyl group, and an isopropyl group; cycloalkyl groups such as a cyclohexyl group; alkenyl groups such as a vinyl group and an allyl group; aryl groups such as a phenyl group and a tolyl group; and groups in which some of the hydrogen atoms of these groups have been substituted with halogen atoms or the like (for example, fluorine-substituted alkyl groups such as a chloromethyl group, a chloropropyl group, a 3,3,3-trifluoropropyl group, and a 3,3,4,4,5,5,6,6,6-nonafluorohexyl group).
[0059] Z 1 and Z 2 are each independently an ethylenically unsaturated bond-containing group and may be —Si(ethylenically unsaturated bond-containing group)(R′)2. The ethylenically unsaturated bond-containing group is preferably a monovalent alkenyl group, more preferably a monovalent alkenyl group having 2 to 4 carbon atoms, and particularly preferably a monovalent vinyl group. R′ is independently a substituted or unsubstituted monovalent hydrocarbon group, and specific examples include alkyl groups such as methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, t-butyl, pentyl, and hexyl; aryl groups such as phenyl, tolyl, and xylyl; and halogenated alkyl groups such as 3-chloropropyl and 3,3,3-trifluoropropyl. Among these, alkyl groups having 1 to 5 carbon atoms are preferred.
[0060]
[0061] In formulas (2) to (4), X, p and R 1 represents X, p and R in the formula (1). 1 It is synonymous with R 3 and R 4 are each independently a substituted or unsubstituted divalent hydrocarbon group which may have one or more atoms selected from oxygen atoms, nitrogen atoms, silicon atoms, and sulfur atoms interposed in the bond, and R 3 and R in formula (3) 4 may each independently be a group represented by the following formula (5) or (6):
[0062]
[0063] In formulas (5) and (6), R 5 is a substituted or unsubstituted monovalent hydrocarbon group, and R 6 is a group containing at least one atom selected from carbon atoms, oxygen atoms, nitrogen atoms, silicon atoms and sulfur atoms.
[0064] R 3 and R 4Although there are no particular limitations on the divalent hydrocarbon group, a divalent hydrocarbon group having 1 to 20 carbon atoms, and particularly preferably 2 to 12 carbon atoms, is preferred. Specific examples include alkylene groups such as methylene, ethylene, propylene, methylethylene, butylene, and hexamethylene; cycloalkylene groups such as cyclohexylene; arylene groups such as phenylene, tolylene, xylylene, naphthylene, and biphenylene; groups in which some of the hydrogen atoms of these groups have been substituted with halogen atoms or the like; and combinations of these substituted or unsubstituted alkylene and arylene groups.
[0065] -(X) p -(Rf-Q) a -Rf-(X) p - is -(O-R 7 ) n - [R 7 represents a perfluoroalkanediyl group, and n represents an integer of 2 or more. 7 may be the same or different.
[0066] R 7 Examples of the perfluoroalkanediyl group represented by the formula (I) include C m F 2m (m is an integer of 2 or more), which may be linear or branched. The number of carbon atoms in the perfluoroalkanediyl group (i.e., m) is, for example, 1 to 10, preferably 2 to 6, more preferably 2 to 4, and particularly preferably 2 to 3.
[0067] n may be 2 or more, for example, 10 or more, preferably 40 or more, and more preferably 70 or more. Also, n is, for example, 300 or less, preferably 200 or less, and more preferably 150 or less.
[0068] -(O-R 7 ) n - may be the same group as Rf below.
[0069] The compound represented by the formula (1) is preferably a compound represented by the following formula (1-1): CH2=CH-(X) p -(Rf-Q) a -Rf-(X)p -CH=CH2 (1-1) [The definitions of each symbol in formula (1-1) are the same as those of each symbol in formula (1)]
[0070] The compound represented by the formula (1-1) is preferably a compound in which a is 0, and in this case, it is represented by the following formula (1-1-1): CH2=CH-(X) p -Rf-(X) p -CH=CH2 (1-1-1) [The definitions of each symbol in formula (1-1-1) are the same as those of each symbol in formula (1)]
[0071] Specific examples of Rf include the following groups: -[CF(Z)OCF2] p -(CF2) r -[CF2OCF(Z)] q - (Z is a fluorine atom or -CF3, and p, q, and r are integers satisfying p≧1, q≧1, 2≦p+q≦200, preferably 2≦p+q≦110, and 0≦r≦6), -CF2CF2OCF2-(CF(CF3)OCF2) s -(CF2) r -(CF2OCF(CF3)) t -CF2OCF2CF2- (r, s, and t are integers satisfying 0≦r≦6, s≧0, t≧0, 0≦s+t≦200, preferably 2≦s+t≦110), -CF(Z)-(OCF(Z)CF2) u -(OCF2) v -OCF(Z)- (Z is a fluorine atom or -CF, and u and v are integers satisfying 1≦u≦100 and 1≦v≦50), -CFCF-[OCFCFCF] w -OCFCF- (where w is an integer satisfying 1≦w≦100.)
[0072] <Compound (b2)> Compound (b2) is a reactive organosilicon compound having a hydrosilyl group, and is a compound other than the elastomer (A). Compound (b2) preferably has two or more, preferably three or more, hydrosilyl groups (Si—H) in one molecule and is capable of addition reacting with at least the ethylenically unsaturated bond in compound (b1). Compound (b2) may be used alone or in combination of two or more.
[0073] Suitable examples of the compound (b2) include the organosilicon compounds described in JP-A Nos. 2003-183402 and 11-116684.
[0074] Examples of compound (b2) include organohydrogenpolysiloxanes having two, preferably three or more, hydrosilyl groups. As the organohydrogenpolysiloxane, organohydrogenpolysiloxanes typically used in addition reaction curable silicone rubber compositions can be used, but compounds represented by the following formula (7) or (8) are particularly preferred:
[0075] Z-CH2CH2-(X) P -Rf-(X) P -CH2CH2-Z...(7) Rf-(X) P -CH2CH2-Z (8) [In formulas (7) and (8), X, p, and Rf have the same meanings as X, p, and Rf in formula (1), and Z is a group represented by the following formula (9) or (10)]
[0076]
[0077] In formulas (9) and (10), R 2 is a substituted or unsubstituted monovalent hydrocarbon group, and b is an integer of 1 to 3 in the compound represented by formula (7) and an integer of 2 to 3 in the compound represented by formula (8). 2The substituted or unsubstituted monovalent hydrocarbon group in is preferably a group having 1 to 8 carbon atoms, and specific examples thereof include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, t-butyl, pentyl, neopentyl, hexyl, heptyl, and octyl; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl; aryl groups such as phenyl, tolyl, and xylyl; aralkyl groups such as benzyl and phenylethyl; and groups in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms such as fluorine, chlorine, or bromine (e.g., chloromethyl, chloropropyl, bromoethyl, 3,3,3-trifluoropropyl, and 3,3,4,4,5,5,6,6,6-nonafluorohexyl).
[0078] <Other Components> In addition to the elastomer (A) and compound (B), the present composition may contain other components that have been conventionally incorporated into sealing materials, as needed, as long as the effects of the present invention are not impaired. Examples of such other components include crosslinking agents (C); crosslinking aids (D); polyol-based compounds; organic pigments such as anthraquinone-based pigments, perylene-based pigments, and dioxazine-based pigments; plasticizers; processing aids; vulcanization accelerators; antioxidants; antioxidants; inorganic fillers; and organic fillers. Each of the other components may be used alone or in combination of two or more.
[0079] <Crosslinking Agent (C)> The elastomer (A) can be crosslinked without using a crosslinking agent (C), but the present composition preferably contains a crosslinking agent (C) appropriate for the type of elastomer (A) used, from the viewpoint of being able to easily obtain a sealing material that is sufficiently crosslinked and has a well-balanced excellent properties in hardness, tensile strength, elongation at break, and 100% Mo. When a crosslinking agent (C) is used, the crosslinking agent (C) used in the present composition may be one type or two or more types.
[0080] As the crosslinking agent (C), any conventionally known crosslinking agent can be used without any particular limitation, and may be appropriately selected depending on the type of elastomer (A) used. For example, when FKM is used, examples of the crosslinking agent include peroxide-based crosslinking agents, polyamine-based crosslinking agents, polyol-based crosslinking agents, and triazine-based crosslinking agents.
[0081] Among these, peroxide-based crosslinking agents are preferred because they do not require the incorporation of an acid acceptor such as magnesium oxide or calcium hydroxide, which can be a source of particle generation in a plasma atmosphere, etc., into the composition, and there is no risk of particle generation during use of the resulting sealing material.
[0082] Examples of peroxide-based crosslinking agents include 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, dicumyl peroxide, 2,4-dichlorobenzoyl peroxide, di-t-butyl peroxide, t-butyldicumyl peroxide, benzoyl peroxide, 2,5-dimethyl-2,5-(t-butylperoxy)hexyne-3, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, and t-butylperoxyisopropyl. Examples of the peroxybenzoate include propyl carbonate, di-(4-t-butylcyclohexyl)peroxydicarbonate, p-chlorobenzoyl peroxide, t-butylperoxy-2-ethylhexanoate, t-butylperoxybenzoate, 1,1-bis(t-butylperoxy)-3,5,5-trimethylcyclohexane, 2,5-dimethylhexane-2,5-dihydroperoxide, α,α-bis(t-butylperoxy)-p-diisopropylbenzene, t-butylperoxybenzene, and t-butylperoxymaleic acid. Among these, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,4-dichlorobenzoyl peroxide, dicumyl peroxide, benzoyl peroxide, and α,α'-bis(t-butylperoxy-m-isopropyl)benzene are preferred, and 2,5-dimethyl-2,5-di(t-butylperoxy)hexane is more preferred.
[0083] When the present composition contains a crosslinking agent (C), the content of the crosslinking agent (C) in the present composition is preferably 0.2 to 4 parts by mass, more preferably 0.2 to 2.5 parts by mass, per 100 parts by mass of the elastomer (A), from the viewpoints that the crosslinking reaction proceeds sufficiently and a sealing material having excellent hardness, tensile strength, elongation at break, and 100% Mo in a well-balanced manner can be easily obtained.
[0084] <Crosslinking aid (D)> In the present composition, the crosslinking agent (C) may be used alone, but when the crosslinking agent (C) is used, it is preferable to use a crosslinking aid (D). As the crosslinking aid (D), a known crosslinking aid may be selected depending on the type of crosslinking agent (C). When the crosslinking aid (D) is used, the crosslinking aid (D) used in the present composition may be one type or two or more types.
[0085] For example, examples of crosslinking aids used when a peroxide-based crosslinking agent is used include triallyl isocyanurate, triallyl cyanurate, trimethallyl isocyanurate, triallyl formal, triallyl trimellitate, N,N'-m-phenylene bismaleimide, dipropargyl terephthalate, diallyl phthalate, tetraallyl terephthalamide, polyfunctional (meth)acrylates such as ethylene glycol di(meth)acrylate and trimethylolpropane tri(meth)acrylate; compounds capable of co-crosslinking by radicals (polyfunctional monomers); metal salts of higher carboxylic acids; polyhydric alcohol (meth)acrylates; and metal (meth)acrylic acid salts. Among these, triallyl isocyanurate is preferred from the viewpoints of excellent reactivity, excellent heat resistance, and the ease with which a sealing material with high hardness and high modulus can be obtained.
[0086] When the present composition contains a crosslinking aid (D), the content of the crosslinking aid (D) in the present composition is preferably 1 part by mass or more, more preferably 2 parts by mass or more, even more preferably 4 parts by mass or more, and preferably 10 parts by mass or less, more preferably 8 parts by mass or less, even more preferably 7 parts by mass or less, and particularly preferably 6 parts by mass or less, per 100 parts by mass of the elastomer (A), from the viewpoints that the crosslinking reaction will proceed sufficiently and a sealing material having excellent hardness, tensile strength, elongation at break, and 100% Mo will be easily obtained. In particular, in order to suppress cracks that may occur in the sealing material under a plasma atmosphere, etc., a radiation-crosslinked sealing material (radiation-treated product) is preferred. In this case, the content of the crosslinking aid (D) in the present composition is preferably 2 parts by mass or more, more preferably 4 parts by mass or more, and preferably 10 parts by mass or less, even more preferably 8 parts by mass or less, per 100 parts by mass of the elastomer (A), from the viewpoints that a sealing material having higher hardness and higher modulus will be easily obtained.
[0087] The mass ratio of the content of the crosslinking aid (D) to the content of the crosslinking agent (C) in the composition (content of crosslinking aid (D) / content of crosslinking agent (C)) is preferably 2 or more, more preferably 4 or more, and even more preferably 6 or more, and is preferably 30 or less, more preferably 20 or less, from the viewpoints that the crosslinking agent (C) can be reacted in just the right amount to easily obtain a sealing material exhibiting desired physical properties, in particular, a sealing material with higher hardness and higher modulus can be easily obtained.
[0088] <Polyol-Based Compound> By using the polyol-based compound, it is possible to easily form a sealing material that has excellent crack resistance in a plasma environment without impairing the performance as a sealing material. When a polyol-based compound is used, the polyol-based compound used in the composition may be one type or two or more types.
[0089] Although a wide variety of conventionally known compounds can be used as the polyol compound, bisphenols are preferred, particularly from the viewpoint of easily obtaining a sealing material with excellent crack resistance. Examples of bisphenols include 2,2-bis(4-hydroxyphenyl)perfluoropropane (bisphenol AF), 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), and bis(4-hydroxyphenyl)sulfone (bisphenol S). Salts of these compounds, such as alkali metal salts and alkaline earth metal salts, may also be used. Among these, bisphenol AF and bisphenol A are preferred, with bisphenol AF being more preferred, particularly from the viewpoint of easily obtaining a sealing material with excellent crack resistance.
[0090] When the present composition contains a polyol-based compound, the content of the polyol-based compound in the present composition is preferably 0.1 to 3 parts by mass, more preferably 0.1 to 2 parts by mass, and even more preferably 0.1 to 1 part by mass, per 100 parts by mass of the elastomer (A), from the viewpoint that a sealing material having excellent crack resistance, small compression set, and excellent vulcanization rate can be easily obtained.
[0091] <Organic Pigment> Suitable examples of the organic pigment include the same organic pigments as those described in WO 2004 / 094527, etc. When an organic pigment is used, the organic pigment used in the present composition may be one type or two or more types.
[0092] <Filler> The inorganic filler and organic filler (hereinafter collectively referred to simply as "filler") are particulate (powdered) components other than the compound (B), crosslinking agent (C), and crosslinking aid (D). When a filler is used, the filler used in the composition may be one type or two or more types.
[0093] Examples of the inorganic filler include carbon black, silica, barium sulfate, titanium oxide, and aluminum oxide. Examples of the organic filler include fluororesins such as PTFE, PFA, FEP, ETFE, and PVDF, polyethylene resins, polyimide resins, silicone resins, and melamine resins.
[0094] When the present composition is used for producing a sealing material in which particle generation is a problem, such as in a plasma atmosphere, the content of the filler is preferably 10 parts by mass or less, more preferably 3 parts by mass or less, per 100 parts by mass of the elastomer (A).
[0095] <Method for Producing the Composition> The composition can be produced by mixing (kneading) the elastomer (A), the compound (B), and, if necessary, the other components, and a production method including the following steps 1 and 2 is preferred. Step 1: A step of reacting the compound (b1) with the compound (b2) to synthesize the compound (B). Step 2: A step of mixing the elastomer (A), the compound (B) obtained in step 1, and, if necessary, the other components.
[0096] The order of mixing the elastomer (A), the compound (B), and the other components is not particularly limited, and they may be mixed (kneaded) sequentially in any order, or may be mixed (kneaded) all at once. However, it is preferable to mix (knead) them sequentially so that the components are uniformly mixed.
[0097] The step 1 can be carried out under the conditions described in the section for compound (B).
[0098] The mixing (kneading) can be carried out using a conventionally known mixer (kneader), for example, an open roll, a Banbury mixer, a twin-screw roll, or a kneader. Depending on the mixer (kneader), the mixing (kneading) may be carried out under heating or cooling, as necessary.
[0099] A sealing material according to one embodiment of the present invention (hereinafter also referred to as "the sealing material") is a sealing material obtained from the composition. Because the sealing material is obtained from the composition, it has a good balance of excellent hardness, tensile strength, elongation at break, and 100% Mo, and further has excellent plasma resistance (radical resistance), crack resistance, compression set, etc.
[0100] The present sealant can be used, for example, as a gasket or packing for various components, and because it exhibits the above-mentioned effects in particular, it can be suitably used as a sealant for semiconductor manufacturing equipment or plasma processing equipment, particularly as a sealant for drive parts such as gate valves used at the openings of plasma processing chamber units. The shape, etc. of the present sealant can be selected appropriately depending on the application.
[0101] The present sealing material does not contain the filler, yet can have the following physical properties. The Shore A hardness (type A durometer hardness) of the present sealing material, measured in accordance with JIS K 6253:2012, is preferably 40 or more. The tensile strength of the present sealing material, measured in accordance with JIS K 6251:2017, is preferably 4 MPa or more. The elongation at break of the present sealing material, measured in accordance with JIS K 6251:2017, is preferably 200% or more. The tensile stress at 100% elongation (100% Mo) of the present sealing material, measured in accordance with JIS K 6251:2017, is preferably 0.5 MPa or more.
[0102] <Method for producing the present sealing material> Specifically, the present sealing material can be produced by molding the present composition. However, it is preferable that the present sealing material is a crosslinked product obtained by a method including a step of crosslinking the present composition (crosslinking step), from the viewpoint of being able to easily obtain a sealing material that is excellent in plasma resistance (radical resistance), crack resistance, non-stickiness, etc., and that is well-balanced with respect to hardness, tensile strength, elongation at break, and 100% Mo.
[0103] When forming a sealing material from the present composition, it is preferable to carry out a separating step in order to improve the efficiency of the molding operation, reduce the defective rate, etc. This separating step is usually carried out using a roll or the like, and is usually also a step of preliminarily forming the present composition into a sheet.
[0104] The sheet obtained in the dividing step is preferably preformed into a desired sealing material shape before the crosslinking step. This preforming may involve directly forming the desired sealing material shape from the sheet obtained in the dividing step, or may involve cutting or extrusion molding the sheet obtained in the dividing step into a rope-like shape (which also has the same meaning as a ribbon-like shape or noodle-like shape), and then forming the resulting rope-like product into the desired sealing material shape.
[0105] The crosslinking step preferably includes a primary crosslinking step and a secondary crosslinking step. The crosslinking step is preferably carried out using a preform having a desired sealing material shape obtained by the preforming step.
[0106] The primary crosslinking step is preferably a step of heating and pressurizing a preformed product having a desired sealing material shape obtained by the preforming step. A specific example of this step is a step of placing the preformed product in a mold and crosslinking it using a heating press or the like under a pressure of about 2 to 15 MPa at a temperature of, for example, 150 to 200°C for, for example, about 5 to 20 minutes.
[0107] The secondary crosslinking step is preferably a step of heating the molded body obtained in the primary crosslinking step, and specifically includes a step of heating the molded body obtained in the primary crosslinking step at normal pressure to reduced pressure using various ovens, preferably a vacuum oven, at a temperature of, for example, 150 to 300°C for 1 to 24 hours, more preferably 3 to 24 hours. This secondary crosslinking step promotes crosslinking, and even if unreacted components remain after the primary crosslinking step, the unreacted components can be decomposed and volatilized, thereby making it possible to obtain a sealing material that emits less gas.
[0108] In the method for producing the present sealant, a step of irradiating with radiation (radiation irradiation step) may be carried out after the crosslinking step, in order to more easily suppress cracks that may occur in the sealant in a plasma atmosphere, etc. The present sealant obtained through this radiation irradiation step can be said to be a radiation-treated product.
[0109] The radiation to be irradiated in the radiation irradiation step is preferably radiation capable of crosslinking the elastomer (A), and examples thereof include X-rays, gamma rays, electron beams, proton beams, neutron beams, heavy particle beams, alpha rays, and beta rays, and among these, gamma rays and electron beams are preferred. The radiation to be irradiated may be one type alone or two or more types.
[0110] When irradiating with radiation, it is desirable to irradiate so that the absorbed dose is preferably 1 to 120 kGy, more preferably 20 to 100 kGy. Irradiating with radiation in such an amount can reduce unreacted components that can become particles or released gases, and can easily produce a sealing material that is excellent in plasma resistance, crack resistance, etc., without excessively lowering the molecular weight of the elastomer (A). The radiation irradiation step may be carried out in two or more stages by changing the conditions.
[0111] Although irradiation with radiation may be performed in air, the presence of oxygen during irradiation may inhibit the crosslinking reaction, resulting in a decrease in the mechanical strength of the resulting sealant and a possibility of the resulting sealant becoming sticky on its surface. For this reason, the radiation irradiation step is preferably performed in an atmosphere of an inert gas such as nitrogen or argon.
[0112] An embodiment of the present invention will be described in more detail with reference to examples, but the present invention is not limited to these.
[0113] Synthesis Example 1 SIFEL X-71-8114A and B (both manufactured by Shin-Etsu Chemical Co., Ltd., neither containing silica), i.e., a compound having a perfluoro skeleton and an ethylenically unsaturated bond, and a reactive organosilicon compound having a hydrosilyl group were reacted at 120°C for 1 hour to synthesize a compound having a perfluoro skeleton (hereinafter also referred to as "compound (B1)"). The ratio of SIFEL X-71-8114A to SIFEL X-71-8114B used was 1:1 by mass. The viscosity of the synthesized compound (B1) at 23°C was measured using a cone-plate viscometer in accordance with JIS Z 8803:2011, a method for measuring viscosity of liquids. The viscosity of compound (B1) was 7000 Pa s. In this specification, the viscosity at 23°C measured using a cone-plate viscometer in accordance with JIS Z 8803:2011, a method for measuring viscosity of liquids, is a value measured using a CP-52 spindle at a temperature of 23°C and a rotation speed of 0.05 rpm, at which the torque stabilizes.
[0114] Synthesis Example 2 SIFEL 8070A and B (both manufactured by Shin-Etsu Chemical Co., Ltd., neither containing silica), i.e., a compound having a perfluoro skeleton with an ethylenically unsaturated bond, and a reactive organosilicon compound having a hydrosilyl group were reacted at 120°C for 1 hour to synthesize a compound having a perfluoro skeleton (hereinafter also referred to as "compound (B2)"). The ratio of SIFEL 8070A to SIFEL 8070B used was 1:1 by mass. The viscosity of the synthesized compound (B2) at 23°C was measured using a cone-plate viscometer in accordance with JIS Z 8803:2011, a method for measuring the viscosity of liquids. The viscosity of compound (B2) was 4000 Pa s.
[0115] Example 1 70 parts by mass of Tecnoflon P959 (manufactured by Solvay, fluorine content: 70% by mass, hereinafter also referred to as "crosslinkable fluoroelastomer (A-1)") and 30 parts by mass of Tecnoflon P757 (manufactured by Solvay, fluorine content: 67% by mass, hereinafter also referred to as "crosslinkable fluoroelastomer (A-2)") were kneaded at a rotation speed of 20 ppm using a 6-inch roll with a roll temperature set to 60°C. 10 parts by mass of compound (B1) were added thereto and kneaded until a uniform appearance was achieved. 6 parts by mass of TAIC (manufactured by Mitsubishi Chemical Corporation, triallyl isocyanurate) were added thereto and kneaded until a uniform appearance was achieved. Next, 1 part by mass of Perhexa 25B (manufactured by NOF Corporation) was added thereto and kneaded until a uniform appearance was achieved, thereby obtaining a block of elastomer composition.
[0116] The obtained bulk elastomer composition was filled into a mold and press-molded using a compression vacuum press at 170°C for 10 minutes under a pressure of 5 MPa (primary crosslinking). The press-molded sheet was then heated at 200°C for 16 hours under reduced pressure in a vacuum oven (vacuum degree: 50 Pa) (secondary crosslinking) to produce a molded product (sealing material).
[0117] Examples 2 to 4, 6 and Comparative Example 1 Molded articles (sealing materials) were prepared in the same manner as in Example 1, except that the components shown in Table 1 were used in the amounts (parts by mass) shown in Table 1.
[0118] Example 5 A bulk elastomer composition was obtained in the same manner as in Example 2. The obtained bulk elastomer composition was filled into a mold and press-molded using a compression vacuum press at 170°C for 10 minutes under a pressure of 5 MPa (primary crosslinking). The press-molded sheet was then heated at 200°C for 16 hours under reduced pressure in a vacuum oven (vacuum degree: 50 Pa) (secondary crosslinking). The secondary crosslinked sheet was then irradiated with radiation to an absorbed dose of 40 kGy, thereby producing a molded product (sealing material).
[0119] Comparative Example 2 70 parts by mass of crosslinkable fluoroelastomer (A-1) and 30 parts by mass of crosslinkable fluoroelastomer (A-2) were kneaded at a rotation speed of 20 ppm using a 6-inch roll with the roll temperature set to 60° C. 10 parts by mass of SIFEL X-71-8114A (manufactured by Shin-Etsu Chemical Co., Ltd., silica-free, viscosity at 23° C. measured in accordance with JIS Z 8803:2011 using a cone-plate viscometer: 2 Pa s) and 10 parts by mass of SIFEL X-71-8114B (manufactured by Shin-Etsu Chemical Co., Ltd., silica-free, viscosity at 23° C. measured in accordance with JIS Z 8803:2011 using a cone-plate viscometer: 3 Pa s) were added thereto, and the mixture was kneaded until the appearance was uniform. To this mixture, 6 parts by mass of TAIC (triallyl isocyanurate, manufactured by Mitsubishi Chemical Corporation) was added, followed by the addition of 1 part by mass of Perhexa 25B (manufactured by NOF Corporation). However, the added components were not mixed uniformly, and a massive elastomer composition could not be obtained.
[0120] Comparative Example 3 70 parts by mass of crosslinkable fluoroelastomer (A-1) and 30 parts by mass of crosslinkable fluoroelastomer (A-2) were kneaded at a rotation speed of 20 ppm using a 6-inch roll with the roll temperature set to 60° C. 10 parts by mass of SIFEL 8070A (manufactured by Shin-Etsu Chemical Co., Ltd., silica-free, viscosity at 23° C. measured in accordance with JIS Z 8803:2011 using a cone-plate viscometer: 2 Pa s) and 10 parts by mass of SIFEL 8070B (manufactured by Shin-Etsu Chemical Co., Ltd., silica-free, viscosity at 23° C. measured in accordance with JIS Z 8803:2011 using a cone-plate viscometer: 3 Pa s) were added thereto, and the mixture was kneaded until the appearance was uniform. To this mixture, 6 parts by mass of TAIC (triallyl isocyanurate, manufactured by Mitsubishi Chemical Corporation) was added, followed by the addition of 1 part by mass of Perhexa 25B (manufactured by NOF Corporation). However, the added components were not mixed uniformly, and a massive elastomer composition could not be obtained.
[0121] <Hardness, Tensile Strength, Elongation at Break, and Tensile Stress at 100% Elongation> Using the molded articles obtained in Examples 1 to 6 and Comparative Example 1, the hardness (Shore A hardness) was measured in accordance with JIS K 6253: 2012, and the tensile strength, elongation at break, and tensile stress at 100% elongation (100% Mo) were measured in accordance with JIS K 6251: 2017. The results are shown in Table 1.
[0122] <Adhesion Strength> In Examples 1 to 6 and Comparative Example 1, O-rings (molded articles) were produced in the same manner as in Examples 1 to 6 and Comparative Example 1, except that a mold capable of molding an O-ring of size AS-214 was used as the mold. The produced O-rings were attached to a flange as shown in FIG. 1 , and the flange was clamped with bolts until it reached a metal-to-metal state. Then, the flange was heated in an electric furnace at a test temperature of 150°C for 72 hours. After 72 hours had elapsed, the flange was quickly removed from the electric furnace and allowed to cool to room temperature (25°C). The adhesive strength was determined by subtracting the force due to the flange's own weight from the maximum force when the flange with the bolts removed was then peeled off at a rate of 300 mm / min. A small adhesive strength value is preferable because the O-ring (molded article) is less likely to adhere to a mating member in contact with the molded article, even when used continuously for a long period of time at high temperatures in, for example, a semiconductor manufacturing process.
[0123] <Plasma Resistance> The plasma resistance (mass reduction rate) of the obtained molded body was measured. Specifically, the measurement was performed as follows. The results are shown in Table 1. Using a flat-plate plasma treatment device with an electrode diameter of 300 mm and an electrode distance of 50 mm, the obtained molded body was irradiated with plasma for 3 hours under conditions of RF 1000 W, CF gas flow rate 10 sccm, O gas flow rate 190 sccm, and vacuum level 1 torr. The obtained molded body was placed 6 cm away from the plasma electrode. Next, the mass of the molded body before and after the test was measured, and the mass reduction rate (%) was calculated using the following formula to evaluate the plasma resistance. The smaller the mass reduction rate, the better the plasma resistance. Mass reduction rate (%) = {(mass of molded body before test - mass of molded body after test) / mass of molded body before test} x 100
[0124] <Processability> In the above examples and comparative examples, the state when obtaining a bulk elastomer composition was evaluated according to the following criteria: ◯: The added components could be uniformly mixed in a short time on the 6-inch roll, and the processability was excellent. △: The added components could be uniformly mixed on the 6-inch roll, but the elastomer composition slipped on the 6-inch roll, and the elastomer composition was likely to come off the 6-inch roll, and it took a long time to obtain a uniform elastomer composition. ×: The added components were not uniformly mixed on the 6-inch roll, and a uniform elastomer composition could not be obtained.
[0125] <Processing time> The processing time was the total time from the start of mastication of the crosslinkable fluoroelastomer on a 6-inch roll until the current value stabilized after adding Perhexa 25B. Generally, when kneading, the current value stabilizes once the added components are uniformly kneaded, so the time when the current value stabilizes can be used as a guide to the completion of kneading and can be used to determine that a uniform composition has been obtained.
[0126]
Claims
1. An elastomer composition comprising: (A) a crosslinkable fluoroelastomer; and (B) a compound having a perfluoro skeleton, the viscosity of which at 23°C is 1,000 to 9,000 Pa·s, as measured using a cone-plate viscometer in accordance with JIS Z 8803:2011, a method for measuring the viscosity of liquids.
2. The elastomer composition according to claim 1, wherein the content of the compound (B) having a perfluoro skeleton is 5 parts by mass or more per 100 parts by mass of the crosslinkable fluoroelastomer (A).
3. The elastomer composition according to claim 1, wherein the compound (B) having a perfluoro skeleton is a reaction product of a compound having a perfluoro skeleton having an ethylenically unsaturated bond and a reactive organosilicon compound having a hydrosilyl group.
4. A method for producing an elastomer composition, comprising the following steps 1 and 2: Step 1: A step of reacting a compound having a perfluoro skeleton having an ethylenically unsaturated bond with a reactive organosilicon compound having a hydrosilyl group to synthesize a compound (B) having a perfluoro skeleton having a viscosity of 1000 to 9000 Pa·s at 23°C measured using a cone-plate viscometer in accordance with the liquid viscosity measurement method of JIS Z 8803:2011. Step 2: A step of mixing the crosslinkable fluoroelastomer (A) with the compound (B) having a perfluoro skeleton obtained in the step 1.
5. The method for producing an elastomer composition according to claim 4, wherein in step 2, the compound (B) having a perfluoro skeleton is used in an amount of 5 parts by mass or more per 100 parts by mass of the crosslinkable fluoroelastomer (A).
6. A sealing material obtained from the elastomer composition according to any one of claims 1 to 3.
7. A method for producing a sealing material, comprising a step of crosslinking the elastomer composition according to any one of claims 1 to 3.
Citation Information
Patent Citations
Hardening composition
JP1999116684A
Hardening composition
JP1999116685A
Fluorine-containing copolymer composition
JP2002097329A
Plasma-resistant fluoroelastomer sealing material
JP2003183402A
Fluorine rubber composition
JP2008056739A