Polymer film and laminate
The polymer film, with a liquid and solid phase-separated structure, addresses the challenge of step followability and heat resistance by ensuring a high phase separation interface ratio and low elastic modulus, effectively preventing delamination and maintaining adhesion during high-temperature soldering.
Patent Information
- Application Number
- PCT/JP2024/005087
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-30
- Filing Date
- 2024-02-14
- Publication Date
- 2024-10-03
AI Technical Summary
Polymer films used in copper-clad laminates face challenges in achieving both excellent step followability and heat resistance, particularly during the reflow soldering process, where delamination can occur due to differences in level and adhesion requirements.
A polymer film with a specific composition where material A is liquid at 260°C and material B is solid at 260°C, undergoing phase separation, with a phase separation interface ratio of 2 or more in the cross-section, and having an elastic modulus of 0.60 MPa or less at 160°C, ensuring both excellent adhesion and flexibility.
The polymer film exhibits enhanced step followability and heat resistance, suppressing bubble growth and peeling during high-temperature processes, thereby maintaining integrity with metal layers.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Polymer Films and Laminates
[0001] The present disclosure relates to polymer films and laminates.
[0002] In recent years, the frequencies used in communication devices have tended to become very high. To suppress transmission loss in the high-frequency band, it has become necessary to lower the relative permittivity and dielectric loss tangent of insulating materials used in circuit boards. Copper-clad laminates are preferably used as components constituting circuit boards, and films are preferably used to manufacture copper-clad laminates.
[0003] For example, International Publication No. 2022 / 202789 describes a polymer film that contains a polymer and a filler and has a phase-separated structure containing at least two phases, each of which has an elastic modulus of 0.01 GPa or more. JP 2019-199612 A describes a resin composition that contains a styrene-based polymer, an inorganic filler, and a curing agent, in which the styrene-based polymer is an acid-modified styrene-based polymer having a carboxy group, the inorganic filler is silica and / or aluminum hydroxide, the particle size of the inorganic filler is 1 μm or less, and the content of the inorganic filler is 20 to 80 parts by mass per 100 parts by mass of the styrene-based polymer.
[0004] Typically, copper-clad laminates are manufactured by laminating copper foil on the surface of a polymer film. Furthermore, wiring boards are manufactured by overlapping a copper-clad laminate and a wiring substrate so that the polymer film in the copper-clad laminate contacts the wiring substrate. When manufacturing a wiring board, from the viewpoint of adhesion, it is required that the polymer film conforms to and deforms to the steps formed on the surface of the wiring substrate. On the other hand, when a polymer film with excellent step conformability to the wiring substrate is used in a copper-clad laminate, delamination may occur during the reflow soldering process performed when mounting electronic components. Therefore, there has been a demand for both step conformability to the wiring substrate and excellent adhesion (i.e., excellent heat resistance) during reflow soldering.
[0005] An object of one embodiment of the present disclosure is to provide a polymer film and a laminate that are excellent in step conformability and heat resistance.
[0006] Means for solving the above problems include the following aspects. <1> A polymer film comprising: a material A that is liquid at 260°C; and a material B that is solid at 260°C; wherein materials A and B are phase-separated; in a cross section along the thickness direction of the polymer film, the ratio of the total length of the phase-separation interface between materials A and B to the length in a direction perpendicular to the thickness direction of the polymer film at a thickness of 50 μm is 2 or more; the elastic modulus at 160°C is 0.60 MPa or less; and the dielectric loss tangent is 0.01 or less. <2> The polymer film according to <1>, wherein one of materials A and B forms a continuous phase and the other forms a dispersed phase, and the dispersed phase has an average length in the minor axis direction of 5 μm or less. <3> The polymer film according to <1> or <2>, wherein one of materials A and B forms a continuous phase and the other forms a dispersed phase, and the dispersed phase has an average length in the major axis direction of 10 μm or less. <4> The polymer film according to any one of <1> to <3>, wherein material A is an elastomer containing a structural unit derived from styrene. <5> The polymer film according to any one of <1> to <4>, wherein material A is at least one selected from the group consisting of a styrene-ethylene-butylene-styrene block copolymer, a styrene-isobutylene-styrene block copolymer, a styrene-ethylene-propylene-styrene copolymer, a styrene-isoprene-styrene block copolymer, and hydrogenated products thereof. <6> The polymer film according to any one of <1> to <5>, wherein material B contains an aromatic polyesteramide. <7> A laminate comprising a layer A and a layer B disposed on at least one surface of the layer A, wherein the layer B comprises a material A that is liquid at 260°C and a material B that is solid at 260°C, wherein the materials A and B are phase-separated, and in a cross section along the thickness direction of the layer B, the ratio of the total length of the phase-separation interface between the materials A and B to the length in a direction perpendicular to the thickness direction of the layer B at a thickness of 50 μm is 2 or more, and the laminate has an elastic modulus at 160°C of 0.60 MPa or less and a dielectric loss tangent of 0.01 or less.
[0007] According to one embodiment of the present disclosure, a polymer film and a laminate having excellent step conformability and heat resistance are provided.
[0008] The contents of the present disclosure are described in detail below. The following description of the constituent elements may be based on a representative embodiment of the present disclosure, but the present disclosure is not limited to such an embodiment. In this specification, the term "to" indicating a numerical range is used to mean that the numerical values before and after it are included as the upper and lower limits. In the numerical ranges described in stages in this disclosure, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Furthermore, in the numerical ranges described in this disclosure, the upper or lower limit of that numerical range may be replaced with a value shown in the examples. Furthermore, in the description of groups (atomic groups) in this specification, a notation that does not specify whether they are substituted or unsubstituted encompasses both unsubstituted and substituted groups. For example, the term "alkyl group" encompasses not only alkyl groups without substituents (unsubstituted alkyl groups) but also alkyl groups with substituents (substituted alkyl groups). In this specification, "(meth)acrylic" is a term used to conceptually encompass both acrylic and methacrylic, and "(meth)acryloyl" is a term used to conceptually encompass both acryloyl and methacryloyl. Furthermore, the term "process" in this specification includes not only an independent process but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. Furthermore, in this disclosure, a combination of two or more preferred aspects is a more preferred aspect. Furthermore, unless otherwise specified, the weight-average molecular weight (Mw) and number-average molecular weight (Mn) in this disclosure are molecular weights determined by a gel permeation chromatography (GPC) analyzer using a TSKgel Super HM-H (trade name of Tosoh Corporation) column, a PFP (pentafluorophenol) / chloroform solvent (mass ratio) = 1 / 2, a differential refractometer, and conversion using polystyrene as a standard substance. The average particle size (e.g., D50) of particles in the present disclosure is measured using a laser diffraction / scattering particle size distribution analyzer, such as the LA-950V2 manufactured by HORIBA.
[0009] [Polymer Film] The polymer film according to the present disclosure comprises a material A that is liquid at 260°C and a material B that is solid at 260°C, wherein materials A and B are phase-separated, and in a cross section along the thickness direction of the polymer film, the ratio of the total length of the phase-separation interface between materials A and B to the length in a direction perpendicular to the thickness direction of the polymer film at a thickness of 50 μm is 2 or more, and the elastic modulus at 160°C is 0.60 MPa or less, and the dielectric loss tangent is 0.01 or less.
[0010] As a result of extensive investigations, the present inventors have found that the above-described structure can provide a polymer film having excellent step-conforming ability and heat resistance. Although the detailed mechanism by which the above-described effects are obtained is unknown, it is speculated as follows.
[0011] In the reflow soldering process performed when mounting electronic components, the polymer film is heated at high temperatures (e.g., 260°C). During this process, the water present in the polymer film becomes supersaturated and diffuses, presumably generating bubble nuclei. Materials A and B are phase-separated, and in a cross section along the thickness direction of the polymer film, if the ratio of the total length of the phase-separation interface between materials A and B to the length in the direction perpendicular to the thickness direction of the polymer film at a thickness of 50 μm is 2 or greater, bubble growth is suppressed, thereby preventing peeling between the polymer film and the metal layer. In other words, the polymer film has excellent heat resistance. Furthermore, since the elastic modulus at 160°C is 0.60 MPa or less, the polymer film has excellent step conformability.
[0012] In contrast, WO 2022 / 202789 and JP 2019-199612 A do not include any description focusing on the length of the phase separation interface in a cross section along the thickness direction of the polymer film.
[0013] <Material A> The polymer film according to the present disclosure includes material A that is liquid at 260°C. Material A may be a low molecular weight compound or a high molecular weight compound as long as it is liquid at 260°C. Material A may be one type only, or two or more types. The fact that the material is liquid at 260°C can be confirmed by the viscosity being 100,000 Pa s or less when heated to 260°C.
[0014] Among these, from the viewpoint of conformability to unevenness, it is preferable that material A be a thermoplastic resin, a thermoplastic elastomer, an uncured or semi-cured product of a thermosetting resin, or an uncured or semi-cured product of a thermosetting elastomer.
[0015] Examples of thermoplastic resins include polyurethane resins, polyester resins, (meth)acrylic resins, polystyrene resins, fluororesins, polyimide resins, fluorinated polyimide resins, polyamide resins, polyamideimide resins, polyetherimide resins, cellulose acylate resins, polyurethane resins, polyether ether ketone resins, polycarbonate resins, polyolefin resins (e.g., polyethylene resins, polypropylene resins, resins made of cyclic olefin copolymers, alicyclic polyolefin resins), polyarylate resins, polyethersulfone resins, polysulfone resins, fluorene ring-modified polycarbonate resins, alicyclic modified polycarbonate resins, and fluorene ring-modified polyester resins.
[0016] Examples of thermoplastic elastomers include elastomers containing structural units derived from styrene (polystyrene-based elastomers), polyester-based elastomers, polyolefin-based elastomers, polyurethane-based elastomers, polyamide-based elastomers, polyacrylic-based elastomers, silicone-based elastomers, polyimide-based elastomers, etc. The thermoplastic elastomer may be a hydrogenated product.
[0017] Examples of polystyrene elastomers include styrene-butadiene-styrene block copolymers (SBS), styrene-isoprene-styrene block copolymers (SIS), polystyrene-poly(ethylene-propylene) diblock copolymers (SEP), polystyrene-poly(ethylene-propylene)-polystyrene triblock copolymers (SEPS), styrene-ethylene-butylene-styrene block copolymers (SEBS), and polystyrene-poly(ethylene / ethylene-propylene)-polystyrene triblock copolymers (SEEPS), styrene-isobutylene-styrene block copolymers (SIBS), and hydrogenated products thereof.
[0018] Among these, from the viewpoints of dielectric loss tangent and step-conforming ability, material A is preferably a thermoplastic elastomer, more preferably an elastomer containing a structural unit derived from styrene, and even more preferably at least one selected from the group consisting of a styrene-ethylene-butylene-styrene block copolymer, a styrene-isobutylene-styrene block copolymer, a styrene-ethylene-propylene-styrene copolymer, a styrene-isoprene-styrene block copolymer, and hydrogenated products thereof.
[0019] From the viewpoint of achieving both conformability to unevenness and processability, the content of material A is preferably 40% by mass to 95% by mass, and more preferably 60% by mass to 90% by mass, based on the total mass of the polymer film.
[0020] The weight average molecular weight of material A is preferably 1,000 or more, more preferably 10,000 or more, and even more preferably 30,000 or more. The upper limit of the weight average molecular weight is, for example, 1,000,000.
[0021] Material A is preferably used as a powder in the production of the polymer film. More preferably, the method for converting material A into a powder includes a swelling step of swelling material A with a liquid medium and a pulverization step of pulverizing the swollen material A.
[0022] The liquid medium used in the swelling step is not particularly limited as long as it is a compound that is liquid at 25°C. Furthermore, when the swelling step is performed under heated conditions, a compound that becomes liquid at the heated temperature can be used. Examples of liquid media include water and organic solvents. The liquid medium may be one type only, or two or more types may be used.
[0023] Examples of organic solvents include alcohols, ketones, alkyl halides, amides, sulfoxides, heterocyclic compounds, hydrocarbons, esters, and ethers.
[0024] In particular, from the viewpoint of swelling the specific polymer in a liquid medium, the absolute value of the difference between the solubility parameter of the liquid medium and the solubility parameter of the polymer having a weight average molecular weight of 1000 or more is 5 MPa. 1/2 ~10 MPa 1/2 Preferably, 6 MPa 1/2 ~8 MPa 1/2 It is more preferable that:
[0025] When two or more liquid media are used, the solubility parameters of the liquid media are weighted average values.
[0026] In this disclosure, the solubility parameter is the Hansen solubility parameter. The Hansen solubility parameter is a solubility parameter introduced by Hildebrand, which is divided into three components: a dispersion term δd, a polar term δp, and a hydrogen bonding term δh, and expressed in a three-dimensional space. In this disclosure, the solubility parameter is expressed as δ (unit: MPa 1/2 ) and the value calculated using the following formula is used: δ (MPa) 1/2 = (δd 2 +δp 2 +δh 2 ) 1/2The dispersion term δd, polar term δp, and hydrogen bond term δh have been extensively determined by Hansen and his successors, and are described in detail in Polymer Handbook (fourth edition), VII-698 to 711. Details of the Hansen solubility parameter values are described in "Hansen Solubility Parameters; A Users Handbook (CRC Press, 2007)" by Charles M. Hansen. The solubility parameter of a polymer can be calculated from the molecular structure of the polymer using the Hoy method described in Polymer Handbook (fourth edition).
[0027] In the swelling step, from the viewpoint of further reducing the particle size by pulverization, the swelling degree of the swollen material A is preferably 1% to 1000%, more preferably 50% to 500%, and even more preferably 100% to 250%.
[0028] In the present disclosure, the swelling degree is calculated by the following method. After swelling the polymer with a liquid medium, about 1 g of a measurement sample is taken from the swollen polymer and weighed. The weighed mass is designated as W1 (g). The measurement sample is dried for 3 hours and the dried measurement sample is weighed. The weighed mass is designated as W0 (g). The swelling degree is calculated by the following formula. The drying temperature when drying the measurement sample is the higher of the boiling point of the liquid medium used to swell the polymer and the glass transition temperature of the polymer. Swelling degree (%) = {(W1 - W0) / W0} x 100
[0029] When material A is swelled with the liquid medium, the temperature of the liquid medium is not particularly limited as long as it is a temperature at which the liquid medium is in a liquid state, and is preferably, for example, 10°C to 60°C.
[0030] The means for pulverizing the swollen material A is not particularly limited, and examples thereof include a combination of a mortar and a pestle, and a pulverizer (for example, a ball mill, a bead mill, a roller mill, a jet mill, a hammer mill, an attritor, etc.).
[0031] After swelling the material A, it may be pulverized at room temperature. However, from the viewpoint of obtaining a powder with a smaller particle size, it is preferable to cool the swollen material A in a temperature environment of −50° C. or less and then pulverize it.
[0032] The temperature to which the swollen material A is cooled is preferably lower than the melting point of the liquid medium, and more preferably lower than the melting point of the liquid medium by at least 10° C. Specifically, the temperature to which the swollen material A is cooled is more preferably −80° C. or lower, and even more preferably −100° C. or lower.
[0033] <Material B> The polymer film according to the present disclosure includes material B that is solid at 260°C. Material B may be a low molecular weight compound or a high molecular weight compound as long as it is solid at 260°C. Material B may be one type or two or more types. The fact that material B is solid at 260°C can be confirmed by the fact that the modulus of elasticity when heated to 260°C is 0.1 MPa or more.
[0034] Examples of material B include thermosetting resins such as liquid crystal polymers, fluororesins, polymers of compounds having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, polyphenylene ether and modified products thereof, aromatic polyether ketone, phenolic resins, epoxy resins, polyimides, cyanate resins, bismaleimide resins, and triazine resins.
[0035] - Liquid Crystal Polymer - From the viewpoint of dielectric loss tangent, it is preferable that material B contains a liquid crystal polymer.
[0036] The type of liquid crystal polymer is not particularly limited, and known liquid crystal polymers can be used. The liquid crystal polymer may be a thermotropic liquid crystal polymer that exhibits liquid crystallinity in a molten state, or a lyotropic liquid crystal polymer that exhibits liquid crystallinity in a solution state. In the case of a thermotropic liquid crystal, it is preferable that the polymer melts at a temperature of 450°C or less.
[0037] Examples of liquid crystal polymers include liquid crystal polyester, liquid crystal polyester amide in which an amide bond is introduced into liquid crystal polyester, liquid crystal polyester ether in which an ether bond is introduced into liquid crystal polyester, and liquid crystal polyester carbonate in which a carbonate bond is introduced into liquid crystal polyester.
[0038] From the viewpoint of liquid crystallinity, the liquid crystal polymer is preferably a polymer having an aromatic ring, and more preferably an aromatic polyester or an aromatic polyester amide.
[0039] Furthermore, the liquid crystal polymer may be a polymer in which an isocyanate-derived bond such as an imide bond, a carbodiimide bond, or an isocyanurate bond is further introduced into an aromatic polyester or an aromatic polyester amide.
[0040] The liquid crystal polymer is preferably a wholly aromatic liquid crystal polymer made using only aromatic compounds as raw material monomers.
[0041] Examples of liquid crystal polymers include the following: 1) A liquid crystal polymer obtained by polycondensation of (i) an aromatic hydroxycarboxylic acid, (ii) an aromatic dicarboxylic acid, and (iii) at least one compound selected from the group consisting of an aromatic diol, an aromatic hydroxyamine, and an aromatic diamine; 2) A liquid crystal polymer obtained by polycondensation of multiple aromatic hydroxycarboxylic acids; 3) A liquid crystal polymer obtained by polycondensation of (i) an aromatic dicarboxylic acid and (ii) at least one compound selected from the group consisting of an aromatic diol, an aromatic hydroxyamine, and an aromatic diamine; 4) A liquid crystal polymer obtained by polycondensation of (i) a polyester such as polyethylene terephthalate and (ii) an aromatic hydroxycarboxylic acid. Here, the aromatic hydroxycarboxylic acid, aromatic dicarboxylic acid, aromatic diol, aromatic hydroxyamine, and aromatic diamine may each independently be replaced with a derivative capable of polycondensation.
[0042] The melting point of the liquid crystal polymer is preferably higher than 260°C, more preferably higher than 260°C and not higher than 350°C, and even more preferably higher than 260°C and not higher than 330°C.
[0043] In the present disclosure, the melting point is measured using a differential scanning calorimeter. For example, it is measured using a product called "DSC-60A Plus" (manufactured by Shimadzu Corporation). The temperature rise rate in the measurement is 10°C / min.
[0044] The weight average molecular weight of the liquid crystal polymer is preferably 1,000,000 or less, more preferably 3,000 to 300,000, even more preferably 5,000 to 100,000, and particularly preferably 5,000 to 30,000.
[0045] From the viewpoint of further reducing the dielectric loss tangent, the liquid crystal polymer preferably contains an aromatic polyesteramide. The aromatic polyesteramide is a resin having at least one aromatic ring and having an ester bond and an amide bond. In particular, from the viewpoint of heat resistance, the aromatic polyesteramide is preferably a wholly aromatic polyesteramide.
[0046] The aromatic polyesteramide is preferably a crystalline polymer. Material B preferably contains a crystalline aromatic polyesteramide. The crystalline aromatic polyesteramide further reduces the dielectric loss tangent. A crystalline polymer refers to a polymer that has a clear endothermic peak rather than a stepwise change in endothermic amount in differential scanning calorimetry (DSC). Specifically, for example, this means that the half-width of the endothermic peak is within 10°C when measured at a heating rate of 10°C / min. Polymers with a half-width exceeding 10°C and polymers in which no clear endothermic peak is observed are considered amorphous polymers and are distinguished from crystalline polymers.
[0047] The aromatic polyester amide preferably contains a structural unit represented by the following formula 1, a structural unit represented by the following formula 2, and a structural unit represented by the following formula 3: 1 -CO-...Formula 1 -CO-Ar 2 -CO-...Formula 2 -NH-Ar 3 -O-...Formula 3 In Formulas 1 to 3, Ar 1 , Ar 2 , and Ar 3each independently represents a phenylene group, a naphthylene group, or a biphenylylene group. Hereinafter, the structural unit represented by formula 1 may also be referred to as "unit 1", etc.
[0048] Unit 1 can be introduced, for example, by using an aromatic hydroxycarboxylic acid as a raw material. Unit 2 can be introduced, for example, by using an aromatic dicarboxylic acid as a raw material. Unit 3 can be introduced, for example, by using an aromatic hydroxylamine as a raw material.
[0049] Here, the aromatic hydroxycarboxylic acid, aromatic dicarboxylic acid, aromatic diol, and aromatic hydroxylamine may each independently be replaced with a derivative capable of undergoing polycondensation.
[0050] For example, by converting the carboxy group to an alkoxycarbonyl group or an aryloxycarbonyl group, aromatic hydroxycarboxylic acids and aromatic dicarboxylic acids can be replaced with aromatic hydroxycarboxylic acid esters and aromatic dicarboxylic acid esters. By converting the carboxy group to a haloformyl group, aromatic hydroxycarboxylic acids and aromatic dicarboxylic acids can be replaced with aromatic hydroxycarboxylic acid halides and aromatic dicarboxylic acid halides. By converting the carboxy group to an acyloxycarbonyl group, aromatic hydroxycarboxylic acids and aromatic dicarboxylic acids can be replaced with aromatic hydroxycarboxylic acid anhydrides and aromatic dicarboxylic acid anhydrides. Examples of polycondensable derivatives of compounds having hydroxy groups, such as aromatic hydroxycarboxylic acids and aromatic hydroxyamines, include those obtained by acylation of the hydroxy group to an acyloxy group (acylated products). For example, by acylation of the hydroxy group to an acyloxy group, aromatic hydroxycarboxylic acids and aromatic hydroxylamines can be replaced with acylated products, respectively. Examples of polycondensable derivatives of aromatic hydroxylamines include those obtained by acylation of the amino group to an acylamino group (acylated products). For example, aromatic hydroxyamines can be replaced with acylated products by acylation of the amino group to convert them into acylamino groups.
[0051] In formula 1, Ar 1 is preferably a p-phenylene group, a 2,6-naphthylene group, or a 4,4'-biphenylylene group, and more preferably a 2,6-naphthylene group.
[0052] Ar 1 When Ar is a p-phenylene group, unit 1 is, for example, a constitutional unit derived from p-hydroxybenzoic acid. 1 When Ar is a 2,6-naphthylene group, unit 1 is, for example, a structural unit derived from 6-hydroxy-2-naphthoic acid. 1is a 4,4'-biphenylylene group, unit 1 is, for example, a constituent unit derived from 4'-hydroxy-4-biphenylcarboxylic acid.
[0053] In formula 2, Ar 2 is preferably a p-phenylene group, an m-phenylene group, or a 2,6-naphthylene group, and more preferably an m-phenylene group.
[0054] Ar 2 When Ar is a p-phenylene group, unit 2 is, for example, a structural unit derived from terephthalic acid. 2 When Ar is an m-phenylene group, unit 2 is, for example, a structural unit derived from isophthalic acid. 2 is a 2,6-naphthylene group, unit 2 is, for example, a structural unit derived from 2,6-naphthalenedicarboxylic acid.
[0055] In formula 3, Ar 3 is preferably a p-phenylene group or a 4,4'-biphenylylene group, and more preferably a p-phenylene group.
[0056] Ar 3 When Ar is a p-phenylene group, unit 3 is, for example, a constitutional unit derived from p-aminophenol. 3 is a 4,4'-biphenylylene group, unit 3 is, for example, a constitutional unit derived from 4-amino-4'-hydroxybiphenyl.
[0057] With respect to the total content of units 1, 2, and 3, the content of units 1 is preferably 30 mol% or more, the content of units 2 is preferably 35 mol% or less, and the content of units 3 is preferably 35 mol% or less. With respect to the total content of units 1, 2, and 3, the content of units 1 is more preferably 30 mol% to 80 mol%, even more preferably 30 mol% to 60 mol%, and particularly preferably 30 mol% to 40 mol%. With respect to the total content of units 1, 2, and 3, the content of units 2 is preferably 10 mol% to 35 mol%, even more preferably 20 mol% to 35 mol%, and particularly preferably 30 mol% to 35 mol%. With respect to the total content of units 1, 2, and 3, the content of units 3 is preferably 10 mol% to 35 mol%, even more preferably 20 mol% to 35 mol%, and particularly preferably 30 mol% to 35 mol%. The total content of each structural unit is the sum of the amounts (moles) of each structural unit, which is calculated by dividing the mass of each structural unit constituting the aromatic polyesteramide by the formula weight of the structural unit.
[0058] The ratio of the content of units 2 to the content of units 3, expressed as [content of units 2] / [content of units 3] (mol / mol), is preferably 0.9 / 1 to 1 / 0.9, more preferably 0.95 / 1 to 1 / 0.95, and even more preferably 0.98 / 1 to 1 / 0.98.
[0059] The aromatic polyesteramide may independently have two or more types of units 1 to 3. The aromatic polyesteramide may also have other structural units in addition to units 1 to 3. The content of other structural units is preferably 10 mol % or less, more preferably 5 mol % or less, based on the total content of all structural units.
[0060] The aromatic polyesteramide is preferably produced by melt-polymerizing raw material monomers corresponding to the structural units that constitute the aromatic polyesteramide.
[0061] The weight average molecular weight of the aromatic polyesteramide is preferably 1,000,000 or less, more preferably 3,000 to 300,000, even more preferably 5,000 to 100,000, and particularly preferably 5,000 to 30,000.
[0062] -Fluororesin- From the viewpoint of heat resistance and mechanical strength, material B may be a fluororesin.
[0063] In the present disclosure, the type of fluororesin is not particularly limited, and known fluororesins can be used.
[0064] Fluorine resins include homopolymers and copolymers containing structural units derived from fluorinated α-olefin monomers, i.e., α-olefin monomers containing at least one fluorine atom, and copolymers containing structural units derived from fluorinated α-olefin monomers and structural units derived from non-fluorinated ethylenically unsaturated monomers reactive with the fluorinated α-olefin monomers.
[0065] Fluorinated α-olefin monomers include CF 2 =CF 2 , CHF=CF 2 , C.H. 2 =CF 2 , CHCl=CHF, CClF=CF 2 , CCl 2 =CF 2 , CClF=CClF, CHF=CCl 2 , C.H. 2 = CClF, CCl 2 = CClF, CF 3 CF = CF 2 , C.F. 3 CF = CHF, CF 3 CH=CF 2 , C.F. 3 CH=CH 2 , CHF 2 CH=CHF, CF 3 CF = CF 2, and perfluoro(C2-C8 alkyl) vinyl ethers (e.g., perfluoromethyl vinyl ether, perfluoropropyl vinyl ether, and perfluorooctyl vinyl ether). Among these, the fluorinated α-olefin monomers include tetrafluoroethylene (CF 2 =CF 2 ), chlorotrifluoroethylene (CClF=CF 2 ), (perfluorobutyl)ethylene, vinylidene fluoride (CH 2 =CF 2 ), and hexafluoropropylene (CF 2 =CFCF 3 ) is preferably at least one monomer selected from the group consisting of: ethylene, propylene, butene, and ethylenically unsaturated aromatic monomers (for example, styrene and α-methylstyrene). The fluorinated α-olefin monomer may be used alone or in combination of two or more types. The non-fluorinated ethylenically unsaturated monomer may be used alone or in combination of two or more types.
[0066] Examples of fluororesins include polychlorotrifluoroethylene (PCTFE), poly(chlorotrifluoroethylene-propylene), poly(ethylene-tetrafluoroethylene) (ETFE), poly(ethylene-chlorotrifluoroethylene) (ECTFE), poly(hexafluoropropylene), poly(tetrafluoroethylene) (PTFE), poly(tetrafluoroethylene-ethylene-propylene), poly(tetrafluoroethylene-hexafluoropropylene) (FEP), poly(tetrafluoroethylene-propylene) (FEPM), poly(tetrafluoroethylene-perfluoropropylene vinyl ether), poly(tetrafluoroethylene-perfluoroalkyl vinyl ether) (PFA) (e.g., poly(tetrafluoroethylene-perfluoropropyl vinyl ether)), polyvinyl fluoride (PVF), polyvinylidene fluoride (PVDF), poly(vinylidene fluoride-chlorotrifluoroethylene), perfluoropolyether, perfluorosulfonic acid, and perfluoropolyoxetane.
[0067] The fluororesin may have a structural unit derived from fluorinated ethylene or fluorinated propylene. The fluororesin may be used alone or in combination of two or more types.
[0068] The fluororesin is preferably FEP, PFA, ETFE, or PTFE. FEP is available from DuPont under the trade name TEFLON FEP, or from Daikin Industries, Ltd. under the trade name NEOFLON FEP. PFA is available from Daikin Industries, Ltd. under the trade name NEOFLON PFA, from DuPont under the trade name TEFLON PFA, or from Solvay Solexis under the trade name HYFLON PFA.
[0069] The fluororesin more preferably contains PTFE. The PTFE may be a PTFE homopolymer, a partially modified PTFE homopolymer, or a combination containing one or both of these. The partially modified PTFE homopolymer preferably contains less than 1 mass% of structural units derived from comonomers other than tetrafluoroethylene, based on the total mass of the polymer.
[0070] The fluororesin may be a crosslinkable fluoropolymer having a crosslinkable group. The crosslinkable fluoropolymer can be crosslinked by a conventionally known crosslinking method. One of the representative crosslinkable fluoropolymers is a fluoropolymer having (meth)acryloyloxy. For example, the crosslinkable fluoropolymer is a fluoropolymer having the formula: H 2 C=CR'COO-(CH 2 ) n -R-(CH 2 ) n -OOCR'=CH 2 In this formula, R is an oligomer chain containing constitutional units derived from fluorinated α-olefin monomers, and R′ is H or —CH 3 and n is 1 to 4. R may be a fluorine-containing oligomer chain containing a structural unit derived from tetrafluoroethylene.
[0071] A crosslinked fluoropolymer network can be formed by exposing a fluoropolymer having (meth)acryloyloxy groups to a free radical source to initiate a radical crosslinking reaction via the (meth)acryloyloxy groups on the fluororesin. The free radical source is not particularly limited, but suitable examples include a photoradical polymerization initiator or an organic peroxide. Suitable photoradical polymerization initiators and organic peroxides are well known in the art. Crosslinkable fluoropolymers are commercially available, for example, Viton B manufactured by DuPont.
[0072] —Polymer of a Compound Having a Cyclic Aliphatic Hydrocarbon Group and a Group Having an Ethylenically Unsaturated Bond— Material B may be a polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond.
[0073] Examples of polymers of compounds having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond include thermoplastic resins having structural units derived from cyclic olefin monomers such as norbornene or polycyclic norbornene monomers.
[0074] The polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond may be a ring-opening polymer of the above-mentioned cyclic olefin or a hydrogenated product of a ring-opening copolymer using two or more kinds of cyclic olefins, or may be an addition polymer of a cyclic olefin and an aromatic compound having an ethylenically unsaturated bond such as a chain olefin or a vinyl group. In addition, a polar group may be introduced into the polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond.
[0075] The polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond may be used alone or in combination of two or more kinds.
[0076] The ring structure of the cycloaliphatic hydrocarbon group may be a monocycle, a fused ring in which two or more rings are fused, or a bridged ring. Examples of the ring structure of the cycloaliphatic hydrocarbon group include a cyclopentane ring, a cyclohexane ring, a cyclooctane ring, an isophorone ring, a norbornane ring, and a dicyclopentane ring. The compound having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond is not particularly limited, and examples thereof include (meth)acrylate compounds having a cycloaliphatic hydrocarbon group, (meth)acrylamide compounds having a cycloaliphatic hydrocarbon group, and vinyl compounds having a cycloaliphatic hydrocarbon group. Among these, (meth)acrylate compounds having a cycloaliphatic hydrocarbon group are preferred. Furthermore, the compound having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond may be a monofunctional ethylenically unsaturated compound or a polyfunctional ethylenically unsaturated compound. The number of cycloaliphatic hydrocarbon groups in the compound having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond may be one or more, and may be two or more. The polymer of a compound having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond may be a polymer obtained by polymerizing at least one compound having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, and may be a polymer of a compound having two or more types of cycloaliphatic hydrocarbon groups and a group having an ethylenically unsaturated bond, or may be a copolymer with another ethylenically unsaturated compound that does not have a cycloaliphatic hydrocarbon group. Furthermore, the polymer of a compound having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond is preferably a cycloolefin polymer.
[0077] -Polyphenylene Ether- Material B may be polyphenylene ether. From the viewpoints of dielectric dissipation factor and heat resistance, the average number of phenolic hydroxyl groups at the molecular terminals of the polyphenylene ether (number of terminal hydroxyl groups) per molecule is preferably 1 to 5, and more preferably 1.5 to 3. The number of terminal hydroxyl groups of the polyphenylene ether can be determined, for example, from the specification value of the polyphenylene ether product. The number of terminal hydroxyl groups is expressed, for example, as the average number of phenolic hydroxyl groups per molecule of all polyphenylene ethers present in 1 mole of the polyphenylene ether. One type of polyphenylene ether may be used alone, or two or more types may be used in combination.
[0078] Examples of polyphenylene ethers include polyphenylene ethers composed of 2,6-dimethylphenol and at least one of a bifunctional phenol and a trifunctional phenol, and poly(2,6-dimethyl-1,4-phenylene oxide). More specifically, the polyphenylene ether is preferably a compound having a structure represented by the formula (PPE).
[0079]
[0080] In formula (PPE), X represents an alkylene group having 1 to 3 carbon atoms or a single bond, m represents an integer of 0 to 20, n represents an integer of 0 to 20, and the sum of m and n represents an integer of 1 to 30. Examples of the alkylene group in X include a dimethylmethylene group.
[0081] When the polyphenylene ether is thermally cured after film formation, the weight average molecular weight (Mw) is preferably 500 to 5,000, and more preferably 500 to 3,000, from the viewpoints of heat resistance and film formability. When the polyphenylene ether is not thermally cured, the weight average molecular weight (Mw) is not particularly limited, but is preferably 3,000 to 100,000, and more preferably 5,000 to 50,000.
[0082] - Aromatic Polyether Ketone - Material B may be an aromatic polyether ketone.
[0083] The aromatic polyether ketone is not particularly limited, and any known aromatic polyether ketone can be used.
[0084] The aromatic polyether ketone is preferably polyether ether ketone.
[0085] Polyether ether ketone is a type of aromatic polyether ketone, and is a polymer in which bonds are arranged in the following order: ether bond, ether bond, and carbonyl bond. Each bond is preferably connected by a divalent aromatic group. The aromatic polyether ketone may be used alone or in combination of two or more types.
[0086] Examples of aromatic polyether ketones include polyether ether ketone (PEEK) having a chemical structure represented by the following formula (P1), polyether ketone (PEK) having a chemical structure represented by the following formula (P2), polyether ketone ketone (PEKK) having a chemical structure represented by the following formula (P3), polyether ether ketone ketone (PEEKK) having a chemical structure represented by the following formula (P4), and polyether ketone ether ketone ketone (PEKEKK) having a chemical structure represented by the following formula (P5).
[0087]
[0088] In terms of mechanical properties, n in each of the formulae (P1) to (P5) is preferably 10 or greater, and more preferably 20 or greater. On the other hand, in terms of ease of production of the aromatic polyether ketone, n is preferably 5,000 or less, and more preferably 1,000 or less. That is, n is preferably 10 to 5,000, and more preferably 20 to 1,000.
[0089] Furthermore, material B may be in a particulate form. When material B is in a particulate form, material B may be organic particles or inorganic particles. When the polymer film contains particulate material B, it is preferable that the polymer film also contains material B that is not particulate.
[0090] Examples of resins constituting the organic particles include polyethylene, polystyrene, urea-formalin filler, polyester, cellulose, acrylic resin, fluororesin, cured epoxy resin, crosslinked benzoguanamine resin, crosslinked acrylic resin, and liquid crystal polymer. The resins constituting the organic particles may be one type or two or more types.
[0091] The organic particles may be fibrous, such as nanofibers, or hollow resin particles.
[0092] Among them, from the viewpoint of dielectric loss tangent and step-conforming ability, the organic particles are preferably fluororesin particles, polyester-based resin particles, polyethylene particles, liquid crystal polymer particles, or nanofibers of cellulose-based resins, more preferably polytetrafluoroethylene particles, polyethylene particles, or liquid crystal polymer particles, and particularly preferably liquid crystal polymer particles. Here, the liquid crystal polymer particles refer to, but are not limited to, a liquid crystal polymer polymer polymerized and pulverized with a pulverizer or the like to obtain a powdered liquid crystal. The preferred embodiments of the liquid crystal polymer constituting the liquid crystal polymer particles are the same as the preferred embodiments of the liquid crystal polymer described above.
[0093] The average particle size of the organic particles is preferably 5 nm to 20 μm, more preferably 100 nm to 10 μm, from the viewpoint of dielectric loss tangent and step-conforming ability.
[0094] Examples of compounds constituting the inorganic particles include BN and Al. 2 O 3 , AlN, TiO 2 , SiO 2 , barium titanate, strontium titanate, aluminum hydroxide, and calcium carbonate. The compound constituting the inorganic particles may be one type or two or more types.
[0095] Among these, as inorganic particles, from the viewpoint of dielectric loss tangent and step-following ability, metal oxide particles or fibers are preferred, silica particles, titania particles, or glass fibers are more preferred, and silica particles or glass fibers are particularly preferred.
[0096] From the viewpoint of dielectric loss tangent and step-conforming ability, the average particle size of the inorganic particles is preferably 5 nm to 20 μm, more preferably 10 nm to 10 μm, even more preferably 20 nm to 1 μm, and particularly preferably 25 nm to 500 nm.
[0097] Furthermore, materials A and B may contain a foaming agent that disappears or decomposes upon heating to release a gas. The foaming agent may be an organic foaming agent or an inorganic foaming agent.
[0098] Examples of organic foaming agents include particles containing an acrylic resin as a main component, particles containing an ethyl cellulose resin as a main component, particles containing a butyral resin as a main component, nitrosamine compounds such as dinitrosopentamethylenetetramine (DPT), azo compounds such as azodicarbonamide (ADCA), and hydrazine compounds such as 4,4'-oxybisbenzenesulfonylhydrazide (OBSH) and hydrazodicarbonamide (HDCA).
[0099] Examples of inorganic foaming agents include bicarbonates such as sodium bicarbonate; carbonates; and combinations of bicarbonates and organic acid salts such as sodium citrate.
[0100] From the viewpoint of heat resistance, the content of material B is preferably 5% by mass to 60% by mass, and more preferably 10% by mass to 40% by mass, based on the total mass of the polymer film.
[0101] The polymer film according to the present disclosure may contain other additives in addition to material A and material B. Known additives can be used as the other additives. Examples of the other additives include a curing agent, a leveling agent, an antifoaming agent, an antioxidant, an ultraviolet absorber, a flame retardant, and a colorant.
[0102] In the polymer film according to the present disclosure, material A and material B are phase-separated. Whether or not phase separation has occurred can be determined by cutting out a cross section of the polymer film along its thickness direction with a microtome and observing it with an optical microscope. If sufficient contrast cannot be obtained with an optical microscope, it can also be determined by observing the elastic modulus distribution with a DFM.
[0103] In a cross section of the polymer film along the thickness direction, at a thickness of 50 μm, the ratio of the total length of the phase separation interface between material A and material B to the length in the direction perpendicular to the thickness direction of the polymer film is 2 or more. The ratio is preferably 20 or more, and more preferably 40 or more. The upper limit of the ratio is not particularly limited and may be, for example, 100, preferably 80 or less, more preferably 70 or less, and even more preferably 60 or less.
[0104] The phase separation interface refers to the interface formed between material A and material B.
[0105] The total length of the phase separation interface is measured by the following method.
[0106] It is preferable that one of material A and material B forms a continuous phase, and the other forms a dispersed phase. The dispersed phase preferably has an average length in the minor axis direction of 5 μm or less, more preferably 3 μm or less. The lower limit of the average length in the minor axis direction is not particularly limited, but is, for example, 0.1 μm. The dispersed phase preferably has an average length in the major axis direction of 10 μm or less, more preferably 5 μm or less. The lower limit of the average length in the major axis direction is not particularly limited, but is, for example, 0.5 μm.
[0107] The length in the long axis direction means the length of the longest part of one dispersed phase separated into island-like phases, and the length in the short axis direction means the length of the shortest part in the direction perpendicular to the long axis direction.
[0108] When the average length in the minor axis direction of the dispersed phase is 5 μm or less, the growth of bubbles is further suppressed when the polymer film is heated at a high temperature (e.g., 260°C), and peeling between the polymer film and the metal layer is further suppressed.
[0109] Furthermore, if the average length in the long axis direction of the dispersed phase is 10 μm or less, when the polymer film is heated at a high temperature (e.g., 260°C), the growth of bubbles is further suppressed, and peeling between the polymer film and the metal layer is further suppressed.
[0110] <Physical Properties of Polymer Film> The polymer film according to the present disclosure has a modulus of elasticity of 0.60 MPa or less, preferably 0.50 MPa or less, and more preferably 0.49 MPa or less at 160° C. The lower limit of the modulus of elasticity at 160° C. is not particularly limited, but is, for example, 0.20 MPa.
[0111] Since the modulus of elasticity at 160° C. is 0.60 MPa or less, the polymer film has excellent conformability to unevenness.
[0112] In the present disclosure, the modulus of elasticity of a polymer film at 160°C is measured by the following method. First, a film cross-section sample (2 mm long x 2 mm wide) is prepared by cutting the surface of the polymer film with a microtome. Next, the 160°C modulus of elasticity of the film cross-section sample is measured as the indentation modulus using a nanoindentation method. The indentation modulus is measured using a microhardness tester (for example, product name "DUH-W201" manufactured by Shimadzu Corporation) by applying a load with a Vickers indenter at a loading rate of 0.28 mN / s, holding a maximum load of 10 mN for 10 seconds, and then unloading at a loading rate of 0.28 mN / s.
[0113] The polymer film according to the present disclosure has a dielectric loss tangent of 0.01 or less, preferably 0.005 or less, and more preferably 0.003 or less. The lower limit of the dielectric loss tangent is not particularly limited, but is, for example, 0.0005.
[0114] In the present disclosure, the dielectric loss tangent is measured by the following method. The dielectric loss tangent is measured at a frequency of 10 GHz by a resonance perturbation method. A 10 GHz cavity resonator (CP531 manufactured by Kanto Electronics Application Development Co., Ltd.) is connected to a network analyzer (E8363B manufactured by Agilent Technology Corporation), a polymer film is inserted into the cavity resonator, and the dielectric loss tangent is measured from the change in resonance frequency before and after insertion for 96 hours in an environment of 25°C temperature and 60% RH.
[0115] The average thickness of the polymer film according to the present disclosure is not particularly limited, but from the viewpoint of the dielectric loss tangent and the ability to conform to unevenness, it is preferably 5 μm to 90 μm, more preferably 10 μm to 70 μm, and particularly preferably 15 μm to 50 μm.
[0116] The average thickness of the polymer film is determined by measuring any five points using an adhesive film thickness meter, for example, an electronic micrometer (product name "KG3001A", manufactured by Anritsu Corporation), and averaging these values.
[0117] [Laminate] A laminate according to the present disclosure includes a layer A and a layer B disposed on at least one surface of layer A, wherein layer B includes a material A that is liquid at 260°C and a material B that is solid at 260°C, wherein materials A and B are phase-separated, and in a cross section along the thickness direction of layer B, at a thickness of 50 μm, the ratio of the total length of the phase-separation interface between materials A and B to the length in a direction perpendicular to the thickness direction of layer B is 2 or more, and the laminate has an elastic modulus at 160°C of 0.60 MPa or less and a dielectric loss tangent of 0.01 or less.
[0118] <Layer A> The laminate according to the present disclosure has a layer A on which a layer B described below is provided. From the viewpoint of making the dielectric loss tangent of the laminate 0.01 or less, the layer A preferably contains a polymer having a dielectric loss tangent of 0.01 or less.
[0119] Layer A may contain only one type of polymer having a dielectric loss tangent of 0.01 or less, or may contain two or more types of polymers.
[0120] The dielectric loss tangent of the polymer having a dielectric loss tangent of 0.01 or less is preferably 0.005 or less, more preferably greater than 0 and 0.003 or less, from the viewpoint of the dielectric loss tangent of the laminate.
[0121] Examples of polymers having a dielectric dissipation factor of 0.01 or less include thermoplastic resins such as liquid crystal polymers, fluororesins, polymers of compounds having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, polyether ether ketone, polyolefin, polyamide, polyester, polyphenylene sulfide, polyether ketone, polycarbonate, polyether sulfone, polyphenylene ether and modified products thereof, and polyether imide; elastomers such as copolymers of glycidyl methacrylate and polyethylene; and thermosetting resins such as phenolic resins, epoxy resins, polyimides, and cyanate resins.
[0122] From the viewpoint of the dielectric loss tangent of the laminate, the polymer having a dielectric loss tangent of 0.01 or less is preferably a liquid crystal polymer. That is, Layer A preferably contains a liquid crystal polymer. Preferred embodiments of the liquid crystal polymer are the same as the preferred embodiments of the liquid crystal polymer that may be contained in the polymer film.
[0123] The layer A may contain a filler in addition to the polymer having a dielectric loss tangent of 0.01 or less.
[0124] The filler may be particulate or fibrous, and may be inorganic or organic particles, specific examples of which are as described above.
[0125] Among these, the filler contained in Layer A is preferably organic particles, more preferably liquid crystal polymer particles, from the viewpoints of the dielectric loss tangent, heat resistance, and step-conforming ability of the laminate.
[0126] Layer A may contain only one type of filler, or may contain two or more types of filler. When Layer A contains a filler, the content of the filler is preferably 30% by mass to 95% by mass, more preferably 50% by mass to 90% by mass, and particularly preferably 60% by mass to 80% by mass, relative to the total mass of Layer A, from the viewpoints of the dielectric loss tangent, heat resistance, and step-following ability of the laminate.
[0127] Layer A may contain other additives in addition to the above-mentioned components. Preferred embodiments of the other additives that may be contained in Layer A are the same as preferred embodiments of the other additives that may be contained in the polymer film according to the present disclosure.
[0128] Layer A may also contain, as other additives, a resin other than a polymer having a dielectric dissipation factor of 0.01 or less. Examples of the resin other than a polymer having a dielectric dissipation factor of 0.01 or less include thermoplastic resins other than liquid crystal polyester, such as polypropylene, polyamide, polyester other than liquid crystal polyester, polyphenylene sulfide, polyether ketone, polycarbonate, polyether sulfone, polyphenylene ether and modified products thereof, and polyetherimide; elastomers such as copolymers of glycidyl methacrylate and polyethylene; and thermosetting resins such as phenolic resins, epoxy resins, polyimide resins, and cyanate resins.
[0129] The total content of other additives in Layer A is preferably 25 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, per 100 parts by mass of the content of the polymer having a dielectric tangent of 0.01 or less.
[0130] The average thickness of Layer A is not particularly limited, but from the viewpoints of the dielectric loss tangent, heat resistance, and suppression of wiring distortion of the laminate, it is preferably 5 μm to 90 μm, more preferably 10 μm to 70 μm, and particularly preferably 15 μm to 50 μm.
[0131] The method for measuring the average thickness of each layer in the laminate according to the present disclosure is as follows.
[0132] The laminate is cut in a plane perpendicular to the plane direction of the laminate, and the thickness is measured at five or more points on the cross section, and the average value of the measurements is taken as the average thickness.
[0133] From the viewpoint of making the dielectric loss tangent of the laminate 0.01 or less, the dielectric loss tangent of Layer A is preferably 0.01 or less, more preferably 0.005 or less, and even more preferably greater than 0 and 0.003 or less.
[0134] <Layer B> The laminate according to the present disclosure has Layer B on at least one surface of Layer A. Layer B includes Material A that is liquid at 260°C and Material B that is solid at 260°C, wherein Materials A and B are phase-separated, and in a cross section along the thickness direction of Layer B, at a thickness of 50 μm, the ratio of the total length of the phase-separation interface between Materials A and B to the length in a direction perpendicular to the thickness direction of Layer B is 2 or more, the elastic modulus at 160°C is 0.60 MPa or less, and the dielectric loss tangent is 0.01 or less.
[0135] Preferred aspects of material A and material B contained in the laminate according to the present disclosure are the same as preferred aspects of material A and material B contained in the polymer film according to the present disclosure. Material A that is liquid at 260°C preferably has an elastic modulus at 260°C of 0.10 MPa or less, and material B that is solid at 260°C preferably has an elastic modulus at 260°C of more than 0.10 MPa.
[0136] A preferred aspect of the ratio of the total length of the phase-separation interface between material A and material B to the length in a direction perpendicular to the thickness direction of layer B at a thickness of 50 μm in a cross section taken along the thickness direction of layer B is the same as a preferred aspect of the ratio of the total length of the phase-separation interface between material A and material B to the length in a direction perpendicular to the thickness direction of the polymer film at a thickness of 50 μm in a cross section taken along the thickness direction of the polymer film according to the present disclosure.
[0137] Layer B may contain other additives in addition to materials A and B. Examples of other additives include the same additives as those that may be contained in the polymer film according to the present disclosure.
[0138] From the viewpoint of conformability to unevenness, the average thickness of Layer B is preferably 5 μm to 50 μm, more preferably 10 μm to 40 μm, and even more preferably 15 μm to 30 μm.
[0139] From the viewpoint of adhesion to the metal layer, the laminate according to the present disclosure preferably further includes a layer C in addition to the layer A and the layer B, and more preferably includes the layer B, the layer A, and the layer C in this order.
[0140] <Layer C> Layer C is preferably an adhesive layer, that is, Layer C is preferably a surface layer (outermost layer).
[0141] From the viewpoint of the dielectric loss tangent of the laminate, it is preferable that Layer C contains at least one polymer.
[0142] The preferred embodiments of the polymer used in Layer C are the same as the preferred embodiments of the polymer used in Layer A having a dielectric loss tangent of 0.01 or less.
[0143] The polymer contained in Layer C may be the same as or different from the polymer contained in Layer A or Layer B. However, from the viewpoint of adhesion between Layer A and Layer C, it is preferable that the polymer be the same as the polymer contained in Layer A.
[0144] Furthermore, the layer C preferably contains an epoxy resin to bond the metal layer and the layer A together.
[0145] The epoxy resin is preferably a crosslinked product of a polyfunctional epoxy compound. A polyfunctional epoxy compound is a compound having two or more epoxy groups. The number of epoxy groups in the polyfunctional epoxy compound is preferably 2 to 4.
[0146] In particular, from the viewpoints of the dielectric loss tangent of the laminate and the adhesiveness to the metal layer, it is preferable that Layer C contains an aromatic polyester amide and an epoxy resin.
[0147] Layer C may contain a filler. Preferred embodiments of the filler used in Layer C are the same as preferred embodiments of the filler used in Layer A.
[0148] Layer C may contain other additives in addition to those described above. Preferred embodiments of the other additives used in Layer C are the same as the preferred embodiments of the other additives used in Layer A, except as described below.
[0149] The average thickness of Layer C is preferably smaller than the average thickness of Layer A from the viewpoints of the dielectric loss tangent of the laminate and adhesion to metal.
[0150] Average thickness T of layer A A and the average thickness T of layer C C T, which is the ratio of A / T C From the viewpoint of the dielectric loss tangent of the laminate and the adhesion to the metal layer, the value of is preferably greater than 1, more preferably 2 to 100, even more preferably 2.5 to 20, and particularly preferably 3 to 10. B and the average thickness T of layer C C T, which is the ratio of B / T C From the viewpoint of the dielectric loss tangent of the laminate and the adhesion to the metal layer, the value of is preferably greater than 1, more preferably 2 to 100, even more preferably 2.5 to 20, and particularly preferably 3 to 10.
[0151] Furthermore, from the viewpoints of the dielectric loss tangent of the laminate and the adhesion to the metal layer, the average thickness of Layer C is preferably 0.1 μm to 20 μm, more preferably 0.5 μm to 15 μm, even more preferably 1 μm to 10 μm, and particularly preferably 2 μm to 8 μm.
[0152] The average thickness of the laminate according to the present disclosure is preferably 6 μm to 200 μm, more preferably 12 μm to 100 μm, and particularly preferably 20 μm to 80 μm, from the viewpoints of strength and electrical properties (characteristic impedance) when laminated with a metal layer.
[0153] The average thickness of the laminate is determined by measuring any five points using an adhesive film thickness meter, for example, an electronic micrometer (product name "KG3001A", manufactured by Anritsu Corporation), and averaging these values.
[0154] The laminate according to the present disclosure preferably has a dielectric loss tangent of 0.01 or less, more preferably 0.005 or less, and even more preferably greater than 0 and 0.003 or less.
[0155] <Method for Producing Laminate> (Film Formation) The method for producing the laminate according to the present disclosure is not particularly limited, and known methods can be used.
[0156] Suitable film-forming methods include, for example, co-casting, multi-layer coating, co-extrusion, etc. Among these, the co-casting method is preferred.
[0157] When the multilayer structure of the laminate is produced by a co-casting method or a multi-layer coating method, it is preferable to carry out the co-casting method or the multi-layer coating method using a layer A-forming composition, a layer B-forming composition, a layer C-forming composition, etc., in which the components of each layer, such as a liquid crystal polymer, are dissolved or dispersed in a solvent.
[0158] Examples of the solvent include halogenated hydrocarbons such as dichloromethane, chloroform, 1,1-dichloroethane, 1,2-dichloroethane, 1,1,2,2-tetrachloroethane, 1-chlorobutane, chlorobenzene, and o-dichlorobenzene; halogenated phenols such as p-chlorophenol, pentachlorophenol, and pentafluorophenol; ethers such as diethyl ether, tetrahydrofuran, and 1,4-dioxane; ketones such as acetone and cyclohexanone; esters such as ethyl acetate and γ-butyrolactone; and ethylene carbonate. nitriles such as acetonitrile and succinonitrile; amides such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone, and urea compounds such as tetramethylurea; nitro compounds such as nitromethane and nitrobenzene; sulfur compounds such as dimethyl sulfoxide and sulfolane; and phosphorus compounds such as hexamethylphosphoramide and tri-n-butylphosphoric acid, and two or more of these may be used.
[0159] As the solvent, a solvent mainly composed of an aprotic compound, particularly an aprotic compound having no halogen atoms, is preferred because it is less corrosive and easier to handle, and the proportion of the aprotic compound in the entire solvent is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and particularly preferably 90% by mass to 100% by mass. Furthermore, as the aprotic compound, an amide such as N,N-dimethylformamide, N,N-dimethylacetamide, tetramethylurea, N-methylpyrrolidone, or an ester such as γ-butyrolactone is preferably used because it easily dissolves the liquid crystal polymer, and N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone are more preferred.
[0160] Furthermore, as the solvent, a solvent containing as a main component a compound having a dipole moment of 3 to 5 is preferred because it easily dissolves the liquid crystal polymer, and the proportion of the compound having a dipole moment of 3 to 5 in the entire solvent is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and particularly preferably 90% by mass to 100% by mass. It is preferable to use a compound having a dipole moment of 3 to 5 as the aprotic compound.
[0161] Furthermore, as the solvent, a solvent containing as a main component a compound having a boiling point of 220°C or lower at 1 atmosphere is preferred because it is easy to remove, and the proportion of the compound having a boiling point of 220°C or lower at 1 atmosphere in the entire solvent is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and particularly preferably 90% by mass to 100% by mass. It is preferable to use a compound having a boiling point of 220°C or lower at 1 atmosphere as the aprotic compound.
[0162] Furthermore, when the laminate manufacturing method according to the present disclosure is produced by the co-casting method, multilayer coating method, co-extrusion method, or the like, a support may be used. Examples of the support include a metal drum, a metal band, a glass plate, a resin film, or a metal foil. Among these, a metal drum, a metal band, or a resin film is preferred. Examples of the resin film include polyimide (PI) film, and examples of commercially available products include U-PIREX S and U-PIREX R manufactured by Ube Industries, Ltd., Kapton manufactured by Toray DuPont Co., Ltd., and IF30, IF70, and LV300 manufactured by SKC Kolon PI. Furthermore, the support may have a surface treatment layer formed on its surface to facilitate peeling. Examples of the surface treatment layer include hard chrome plating, fluororesin, and the like. The average thickness of the support is not particularly limited, but is preferably 25 μm to 75 μm, more preferably 50 μm to 75 μm.
[0163] The method for removing at least a part of the solvent from the cast or coated film-like composition (coating film) is not particularly limited, and any known drying method can be used.
[0164] (Stretching) The laminate according to the present disclosure can be appropriately combined with stretching in order to control molecular orientation and adjust the thermal expansion coefficient and mechanical properties. The stretching method is not particularly limited, and known methods can be used. The stretching may be performed in a solvent-containing state or in a dry film state. Stretching in a solvent-containing state may be performed by gripping the laminate and stretching, or by utilizing autogenous shrinkage due to drying without stretching. Stretching is particularly effective for improving breaking elongation and breaking strength when the film brittleness has decreased due to the addition of an inorganic filler or the like.
[0165] The laminate according to the present disclosure can be used for various purposes, and in particular, can be suitably used as a film for electronic components such as printed wiring boards, and can be more suitably used for flexible printed circuit boards. The laminate according to the present disclosure can also be suitably used as a liquid crystal polymer film for metal bonding.
[0166] The present disclosure will be explained in more detail below with reference to examples. The materials, amounts used, ratios, processing details, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present disclosure. Therefore, the scope of the present disclosure is not limited to the specific examples shown below.
[0167] Details of the materials used in the preparation of the polymer film and laminate are as follows.
[0168] <<Layer B>> <Material A> A1: Frozen and pulverized hydrogenated styrene-isobutylene-styrene block copolymer (product name "SIBSTAR103T-UL", manufactured by Kaneka Corporation) swollen with N-methylpyrrolidone, average particle size 5.0 μm (D50) A2: Jet mill pulverized hydrogenated styrene-ethylene-butylene-styrene block copolymer (product name "Tuftec M1913", manufactured by Asahi Kasei Chemicals Corporation), average particle size 5.0 μm (D50)
[0169] <Material B> P1: Aromatic polyesteramide prepared according to the following production method
[0170] -Synthesis of aromatic polyesteramide P1- A reactor equipped with a stirrer, torque meter, nitrogen gas inlet tube, thermometer, and reflux condenser was charged with 940.9 g (5.0 mol) of 6-hydroxy-2-naphthoic acid, 415.3 g (2.5 mol) of isophthalic acid, 377.9 g (2.5 mol) of acetaminophen, and 867.8 g (8.4 mol) of acetic anhydride. The gas inside the reactor was replaced with nitrogen gas, and then the mixture was heated from room temperature (23°C, the same applies hereinafter) to 140°C over 60 minutes while stirring under a nitrogen gas stream, and refluxed at 140°C for 3 hours. Next, while distilling off by-product acetic acid and unreacted acetic anhydride, the mixture was heated from 150°C to 300°C over 5 hours and held at 300°C for 30 minutes. The contents were then removed from the reactor and cooled to room temperature. The resulting solid was pulverized in a grinder to obtain powdered aromatic polyesteramide P1a. The flow initiation temperature of the aromatic polyesteramide P1a was 193°C. The aromatic polyesteramide P1a was a wholly aromatic polyesteramide. The aromatic polyesteramide P1a was heated from room temperature to 160°C over 2 hours and 20 minutes under a nitrogen atmosphere, then heated from 160°C to 180°C over 3 hours and 20 minutes, and held at 180°C for 5 hours to undergo solid-state polymerization, followed by cooling. The mixture was then pulverized in a grinder to obtain a powdered aromatic polyesteramide P1b. The flow initiation temperature of the aromatic polyesteramide P1b was 220°C. The aromatic polyesteramide P1b was heated from room temperature to 180°C over 1 hour and 25 minutes under a nitrogen atmosphere, then heated from 180°C to 255°C over 6 hours and 40 minutes, and held at 255°C for 5 hours to undergo solid-state polymerization, followed by cooling to obtain a powdered aromatic polyesteramide P1. The flow initiation temperature of the aromatic polyesteramide P1 was 302°C. The melting point of the aromatic polyesteramide P1 was measured using a differential scanning calorimeter and found to be 311° C. The dielectric dissipation factor of the aromatic polyesteramide P1 was 0.003.
[0171] <<Layer A>> <Polymer> Aromatic polyester amide P1 described above <Filler> F1: Liquid crystal polymer particles prepared according to the following production method
[0172] -Synthesis of Liquid Crystal Polymer Particles F1- A reactor equipped with a stirrer, torque meter, nitrogen gas inlet tube, thermometer, and reflux condenser was charged with 1,034.99 g (5.5 mol) of 2-hydroxy-6-naphthoic acid, 89.18 g (0.41 mol) of 2,6-naphthalenedicarboxylic acid, 236.06 g (1.42 mol) of terephthalic acid, 341.39 g (1.83 mol) of 4,4-dihydroxybiphenyl, and potassium acetate and magnesium acetate as catalysts. After the gas inside the reactor was replaced with nitrogen gas, acetic anhydride (1.08 molar equivalents relative to the hydroxyl groups) was further added. Under a nitrogen gas stream, the temperature was raised from room temperature to 150°C over 15 minutes with stirring, and refluxed at 150°C for 2 hours. Next, the temperature was raised from 150°C to 310°C over 5 hours while distilling off the by-product acetic acid and unreacted acetic anhydride. The polymer was removed and cooled to room temperature. The obtained polymer was heated from room temperature to 295°C over 14 hours and solid-state polymerized at 295°C for 1 hour. After solid-state polymerization, it was cooled to room temperature over 5 hours. The obtained liquid crystalline polyester was pulverized using a jet mill (Kurimoto Iron Works, Ltd., "KJ-200") to obtain liquid crystalline polymer particles F1. The liquid crystalline polymer particles F1 had a median diameter (D50) of 7 μm, a dielectric dissipation factor of 0.0007, and a melting point of 334°C.
[0173] <Copper Foil> M1: Copper foil with product name "CF-T9DA-SV-18" manufactured by Fukuda Metal Foil & Powder Co., Ltd., having an average thickness of 18 μm, on the treated side of which a 3 μm-thick polymer layer was formed by the following method. - Formation of Polymer Layer - 8 parts by mass of aromatic polyesteramide P1 was added to 92 parts by mass of N-methylpyrrolidone and stirred at 140°C for 4 hours under a nitrogen atmosphere to obtain a solution of aromatic polyesteramide P1 (solid content concentration 8% by mass). A solution was prepared by mixing 9.96 parts by mass of the aromatic polyesteramide P1 solution with 0.04 parts by mass of an aminophenol-type epoxy resin (product name "jER630" manufactured by Mitsubishi Chemical Corporation). The obtained solution was applied to the treated side of the copper foil using a bar coater and dried at 40°C for 4 hours to remove the solvent from the coating, yielding a copper foil having a 3 μm-thick polymer layer. M2: Product name "MT18FL", manufactured by Mitsui Mining & Smelting Co., Ltd., average thickness 1.5 μm, with 18 μm carrier foil M3: Product name "CF-T49A-DS-18", manufactured by Fukuda Metal Foil & Powder Co., Ltd., average thickness 18 μm
[0174] Next, in order to prepare a polymer film and a laminate, a solution for forming Layer A and a solution for forming Layer B were prepared. The polymer film was prepared using the solution for forming Layer B.
[0175] —Preparation of Layer A Forming Solution— The polymers and fillers shown in Table 1 were mixed in the amounts (% by mass) shown in Table 1, and N-methylpyrrolidone was added to adjust the solids concentration to 25% by mass, thereby obtaining a layer A forming solution.
[0176] —Preparation of Layer B Forming Solution— Materials A and B shown in Table 1 were mixed in the amounts (mass %) shown in Table 1, and N-methylpyrrolidone was added to adjust the solids concentration to 20 mass %, thereby obtaining a layer B forming solution.
[0177] [Preparation of Polymer Films Having a Copper Layer (Single-Sided Copper-Clad Laminate)] -Films 2 to 12- The obtained Layer A-forming solution and Layer B-forming solution were fed into a multilayer slot die, and the flow rate was adjusted so that Layer A was positioned on the copper foil side shown in Table 1, and the average thickness after drying was the thickness shown in Table 1. The solvent was removed from the coating by drying at 40°C for 4 hours. Further, the temperature was raised from room temperature to 300°C at a rate of 1°C / min in a nitrogen atmosphere, and a heat treatment was performed in which the temperature was maintained at 300°C for 2 hours, thereby obtaining a laminate (single-sided copper-clad laminate) in which the copper foil, Layer A, and Layer B were laminated in this order.
[0178] -Film 1- The solution for forming Layer B was applied onto a support (product name "Nitoflon #900UL", manufactured by Nitto Denko Corporation, average thickness 50 μm). The solution was dried at 40°C for 4 hours to remove the solvent from the coating, and a polymer film with a support was obtained. Note that for evaluation of the cross section, the 160°C elastic modulus, and the dielectric loss tangent, the support was peeled off, and the sample was further heat-treated by increasing the temperature from room temperature (25°C) to 300°C at a rate of 1°C / min in a nitrogen atmosphere and maintaining it at 300°C for 2 hours.
[0179] -Film A, Film B- The obtained solution for forming Layer A was fed into a slot die and coated onto the copper foil shown in Table 1, adjusting the flow rate so that the average thickness after drying would be the thickness shown in Table 1. The solvent was removed from the coating by drying at 40°C for 4 hours, yielding a polymer film (single-sided copper-clad laminate) having a copper layer. Note that for evaluation of the dielectric loss tangent, a sample was used that had been further heat-treated by increasing the temperature from room temperature (25°C) to 300°C at a rate of 1°C / min in a nitrogen atmosphere and maintaining it at 300°C for 2 hours.
[0180] -Film C- As Film C, an LCP film (product name "Vextar CTQ", manufactured by Kuraray Co., Ltd., average thickness 50 μm) was used, and the treated surface of the copper foil described in Table 1 was laminated at 300°C using a thermocompression bonding machine to obtain a polymer film having a copper layer (single-sided copper-clad laminate).
[0181] [Preparation of Double-Sided Copper-Clad Laminates] The copper foil, first film, and second film listed in Table 2 were laminated in the following order: copper foil / second film / first film. In Examples 1 to 3, a vacuum laminator was used to laminate the second film on the side opposite the support to the first film on the side opposite the copper foil. After peeling off the support from the second film, the film was heated from room temperature to 300°C at a rate of 1°C / min in a nitrogen atmosphere and then held at 300°C for 2 hours to obtain a laminate (single-sided copper-clad laminate) in which the copper foil, first film, and second film were laminated in this order. Furthermore, the treated side of the copper foil was in contact with layer B of the second film, and the copper foil of the first film was the outermost layer. In Examples 4 to 12 and Comparative Examples 1 and 2, the copper foil was laminated on the first film on the treated side so that it was in contact with layer B of the first film. A lamination process was performed for 1 minute using a laminator (product name "Vacuum Laminator V-130", manufactured by Nikko Materials Co., Ltd.) at 140°C and a lamination pressure of 0.4 MPa to obtain a precursor of a double-sided copper-clad laminate. Subsequently, the obtained double-sided copper-clad laminate was thermocompression bonded for 60 minutes using a thermocompression bonding machine (product name "MP-SNL", manufactured by Toyo Seiki Seisakusho, Ltd.) at 230°C and 4 MPa to produce a double-sided copper-clad laminate.
[0182] [Preparation of wiring board] -Preparation of substrate A with wiring pattern- Copper foil (product name "CF-T9DA-SV-18", average thickness 18 μm, manufactured by Fukuda Metal Foil & Powder Co., Ltd.) and a liquid crystal polymer film (product name "CTQ-50", average thickness 50 μm, manufactured by Kuraray Co., Ltd.) were prepared as a substrate. The copper foil, substrate, and copper foil were stacked in this order so that the treated surface of the copper foil was in contact with the substrate. Using a laminator (product name "Vacuum Laminator V-130", manufactured by Nikko Materials Co., Ltd.), a lamination process was performed for 1 minute under conditions of 140°C and a lamination pressure of 0.4 MPa, to obtain a precursor of a double-sided copper-clad laminate. Next, using a thermocompression bonding machine (product name "MP-SNL", manufactured by Toyo Seiki Seisakusho, Ltd.), the obtained precursor of the double-sided copper-clad laminate was thermocompressed for 10 minutes under conditions of 300 ° C and 4.5 MPa to produce a double-sided copper-clad laminate. The surfaces of the copper foil on both sides of the double-sided copper-clad laminate were roughened, and a dry film resist was attached. After exposure and development so that the wiring pattern remained, etching was performed, and the dry film was then removed to produce a substrate A with a wiring pattern having a line / space of 100 μm / 100 μm including a ground line and three pairs of signal lines on both sides of the substrate. The length of the signal line was 50 mm, and the width was set so that the characteristic impedance was 50 Ω.
[0183] - Preparation of substrate B with wiring pattern - Copper foil (product name "MT18FL", average thickness 1.5 μm, with carrier copper foil (thickness 18 μm), manufactured by Mitsui Mining & Smelting Co., Ltd.) and a liquid crystal polymer film (product name "CTQ-50", average thickness 50 μm, manufactured by Kuraray Co., Ltd.) were prepared as a substrate. The copper foil and the substrate were stacked in this order so that the treated surface of the copper foil was in contact with the substrate. Using a laminator (product name "Vacuum Laminator V-130", manufactured by Nikko Materials Co., Ltd.), a lamination treatment was performed for 1 minute under conditions of 140°C and a lamination pressure of 0.4 MPa, to obtain a precursor of a single-sided copper-clad laminate. Next, using a thermocompression bonding machine (product name "MP-SNL", manufactured by Toyo Seiki Seisakusho, Ltd.), the obtained precursor of the single-sided copper-clad laminate was thermocompressed for 10 minutes under conditions of 300 ° C and 4.5 MPa to produce a single-sided copper-clad laminate. The carrier copper foil on the side opposite the substrate of the single-sided copper-clad laminate was peeled off, and the surface of the exposed 1.5 μm copper foil was roughened and laminated with a dry film resist. After pattern exposure and development, the areas where the resist pattern was not located were plated. Furthermore, the dry film resist was peeled off, and the copper exposed by the peeling process was removed by flash etching to produce a substrate B with a wiring pattern having a line / space of 20 μm / 20 μm.
[0184] -Preparation of wiring board- The prepared substrate with wiring pattern was superimposed on the layer B side of the prepared single-sided copper-clad laminate, and a wiring board was obtained by hot pressing for 1 hour under conditions of 160°C and 4 MPa. The obtained wiring board had a wiring pattern (ground line and signal line) embedded therein, and when substrate A with wiring pattern was used, the thickness of the wiring pattern was 18 μm, and when substrate B with wiring pattern was used, the thickness of the wiring pattern was 12 μm.
[0185] <<Evaluation>> The produced wiring boards were subjected to the following measurements and evaluations, and the results are shown in Table 1.
[0186] <<Measurement Method>> [Elastic Modulus at 160°C] The double-sided copper-clad laminate was etched to expose Layer B. The elastic modulus of the exposed area was then measured as the indentation modulus using a nanoindentation method. The indentation modulus was measured using a microhardness tester (product name "DUH-W201", manufactured by Shimadzu Corporation) by applying a load with a Vickers indenter at a loading rate of 0.28 mN / s, holding a maximum load of 10 mN for 10 seconds, and then unloading at a loading rate of 0.28 mN / s.
[0187] [Dielectric loss tangent] The copper foil of a double-sided copper-clad laminate was removed with an aqueous solution of ferric chloride, washed with pure water, and dried to obtain a polymer film. The dielectric loss tangent was measured using a resonance perturbation method at a frequency of 10 GHz. A 10 GHz cavity resonator (Kanto Electronics Application Development Co., Ltd., CP531) was connected to a network analyzer (Agilent Technology, Inc., E8363B). The polymer film was inserted into the cavity resonator, and the dielectric loss tangent of the polymer film was measured from the change in resonance frequency before and after insertion for 96 hours under an environment of 25°C and 60% RH.
[0188] [Cross-Section Evaluation of Layer B] - Ratio of the total length of the phase-separation interface between material A and material B to the length in the direction perpendicular to the thickness direction of the polymer film at a thickness of 50 μm ("Ratio T" in the table) - A cross section along the thickness direction of the polymer film was cut out with a microtome and observed using an optical microscope to observe the phase-separation structure of layer B. From the obtained image, the phase-separation shapes of material A and material B were determined, and the length of the outline was taken as the length of the phase-separation interface between material A and material B. The length of the phase-separation interface was normalized by the thickness of the polymer film and taken as the length at a thickness of 50 μm. The determined length was divided by the length in the direction perpendicular to the thickness direction of the polymer film to calculate the ratio T.
[0189] - Minor axis length (in the table, "minor axis length") and major axis length (in the table, "major axis length") of the dispersed phase - A cross section along the thickness direction of the polymer film was cut out with a microtome and observed with an optical microscope to observe the phase-separated structure of Layer B. From the obtained image, the phase-separated shapes of Material A and Material B were observed, and the shortest length of the island-shaped portions was taken as the minor axis length and the longest length as the major axis length. The average length was calculated as the average of a data group obtained by cutting out three arbitrary locations with a microtome, observing five fields of view for each section, and removing 20% of the data from the top and bottom of all the lengths obtained.
[0190] <<Evaluation Method>> [Step Conformability] The wiring board was cut in the thickness direction with a microtome, and the cross section was observed with an optical microscope. The length L of the gap occurring in the in-plane direction between layer B and the wiring pattern was measured. The average value for 10 locations was calculated. The evaluation criteria are as follows: A: No gap was observed. B: The average value of L was less than 0.5 μm. C: The average value of L was 0.5 μm or more and less than 1 μm. D: The average value of L was 1 μm or more.
[0191] [Heat Resistance] The prepared double-sided copper-clad laminate was cut into a size of 30 mm x 30 mm to prepare an evaluation sample. The evaluation sample was treated for 168 hours in a thermo-hygrostat chamber at a temperature of 85°C and a relative humidity of 85%. The evaluation sample was then placed in an oven set to 260°C and heated for 15 minutes. After heating, the evaluation sample was cut with a razor, and the cross section was observed under an optical microscope to evaluate the state of peeling. A: No peeling was observed between Layer B and the copper foil. B: Peeling was observed between Layer B and the copper foil with a width of 0.5 mm or less. C: Peeling was observed between Layer B and the copper foil with a width of more than 0.5 mm and 1 mm or less. D: Peeling was observed between Layer B and the copper foil with a width of more than 1 mm.
[0192] The measurement results and evaluation results are shown in Table 1. In Film 3, materials A and B did not undergo phase separation, so "-" is entered in the column relating to the dispersed phase.
[0193]
[0194]
[0195] As shown in Table 2, Examples 1 to 12 contain material A that is liquid at 260°C and material B that is solid at 260°C, and material A and material B are phase-separated. In a cross section along the thickness direction of the polymer film, the ratio of the total length of the phase-separated interface between material A and material B to the length in the direction perpendicular to the thickness direction of the polymer film at a thickness of 50 μm is 2 or more. The elastic modulus at 160°C is 0.60 MPa or less, and the dielectric dissipation factor is 0.01 or less, and therefore, the film has excellent step conformability and heat resistance.
[0196] On the other hand, in Comparative Example 1, materials A and B did not undergo phase separation, and in a cross section along the thickness direction of the polymer film, the ratio of the total length of the phase separation interface between materials A and B to the length in the direction perpendicular to the thickness direction of the polymer film at a thickness of 50 μm was less than 2, and therefore it was found that the heat resistance was poor.
[0197] In Comparative Example 2, the modulus of elasticity of the polymer film at 160° C. was more than 0.60 MPa, and it was found that the conformability to unevenness was poor.
[0198] The disclosures of Japanese Patent Application No. 2023-051606, filed on March 28, 2023, and Japanese Patent Application No. 2023-108854, filed on June 30, 2023, are incorporated herein by reference in their entirety. In addition, all documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually indicated to be incorporated by reference.
Claims
1. A polymer film comprising: material A which is liquid at 260°C; and material B which is solid at 260°C; said material A and said material B are phase-separated; in a cross section along the thickness direction of the polymer film, the ratio of the total length of the phase-separated interface between said material A and said material B to the length in the direction perpendicular to the thickness direction of the polymer film at a thickness of 50 μm is 2 or more; the elastic modulus at 160°C is 0.60 MPa or less; and the dielectric loss tangent is 0.01 or less.
2. The polymer film according to claim 1, wherein one of material A and material B forms a continuous phase and the other forms a dispersed phase, and the dispersed phase has an average length in the minor axis direction of 5 μm or less.
3. A polymer film according to claim 1 or 2, wherein one of material A and material B forms a continuous phase and the other forms a dispersed phase, and the dispersed phase has an average length in the major axis direction of 10 μm or less.
4. The polymer film according to claim 1 or 2, wherein material A is an elastomer containing structural units derived from styrene.
5. The polymer film according to claim 1 or 2, wherein material A is at least one selected from the group consisting of a styrene-ethylene-butylene-styrene block copolymer, a styrene-isobutylene-styrene block copolymer, a styrene-ethylene-propylene-styrene copolymer, a styrene-isoprene-styrene block copolymer, and hydrogenated products thereof.
6. The polymer film of claim 1 or claim 2, wherein material B comprises an aromatic polyester amide.
7. A laminate comprising a layer A and a layer B disposed on at least one surface of the layer A, the layer B comprising a material A that is liquid at 260°C and a material B that is solid at 260°C, the materials A and B being phase-separated, the ratio of the total length of the phase-separation interface between the materials A and B to the length in the direction perpendicular to the thickness direction of the layer B at a thickness of 50 μm in a cross section along the thickness direction of the layer B being 2 or more, the elastic modulus at 160°C being 0.60 MPa or less, and the dielectric tangent being 0.01 or less.
Citation Information
Patent Citations
Polymer film and method for producing the same, and laminate and method for manufacturing the same
JP2023020690A
Multilayer film and copper-clad laminate
JP2023029306A
Adhesive composition, adhesive sheet, laminate and printed wiring board
JP6981583B1
Low dielectric resin composition, molded article, film, multilayer film and flexible printed wiring board
WO2020218405A1
Polymer film, multilayer body and method for producing same
WO2022163776A1