Silicon nitride powder and resin composition using same

The use of silicon nitride powder with specific particle characteristics in resin compositions addresses the challenges of moldability and curability by increasing shear rate dependence of viscosity, enhancing both moldability and curability in electronic component heat dissipation applications.

WO2024202734A1PCT designated stage expired Publication Date: 2024-10-03SUMITOMO CHEM CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/006297
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-02-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing resin compositions used for heat dissipation between electronic components and heat sinks lack moldability and curability, particularly in narrow gaps, due to insufficient shear rate dependence of viscosity, which can lead to spillage and damage to surrounding components.

Method used

A silicon nitride powder with specific particle characteristics, such as a minimum angle θ of less than 106.2° and a cumulative particle size distribution ratio of D90/D50 less than 4.8, is used as a filler to increase the shear rate dependence of the viscosity of the resin composition, enabling both excellent moldability and curability.

Benefits of technology

The silicon nitride powder enhances the viscosity's dependence on shear rate, allowing for effective filling of narrow gaps during molding and maintaining shape post-curing, thereby improving moldability and curability of the resin composition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024006297_03102024_PF_FP_ABST
    Figure JP2024006297_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a silicon nitride powder to be used as a filler for a resin composition, the silicon nitride powder being capable of increasing shear rate dependency of viscosity of a mixture with a resin. Provided is a silicon nitride powder containing a plurality of silicon nitride particles, wherein, in each silicon nitride particle, if straight lines are drawn, the straight lines passing through a point on an outer shape in a plan view and extending respectively in the left and right directions of the point with a determination coefficient R2 of more than 0.98 and 1.00 or less, and the angle formed by the straight lines in the left and right directions is referred to as θ and the minimum angle θ in each silicon nitride particle is referred to as the minimum angle θmin, then the average value θave-min of the minimum angle θmin is less than 106.2°.
Need to check novelty before this filing date? Find Prior Art

Description

Silicon nitride powder and resin composition using same

[0001] The present disclosure relates to a silicon nitride powder and a resin composition using the same.

[0002] Heat generated by passing current through an electronic component is dissipated via a heat sink. To improve heat dissipation efficiency, a technique for filling the space between the electronic component and the heat sink with a heat dissipation material is known. One heat dissipation material is a resin composition containing a resin and inorganic particles, and it is known that silicon nitride powder can be used as the inorganic particles (see, for example, Patent Document 1).

[0003] Patent Document 1 discloses a low-aluminum spherical β-silicon nitride powder for use as a filler in electronic packaging materials. The silicon nitride powder is characterized by a sphericity of 0.5 to 0.99, an Al impurity content of less than 500 ppm, and a particle size range of 0.5 μm to 50 μm.

[0004] Patent Document 2 discloses a method for producing silicon nitride powder suitable for producing silicon nitride sintered bodies, and silicon nitride powder obtained by said method. The silicon nitride powder has an average particle size of 1 to 50 μm, a metal oxide content of 0 to 10 wt %, and an impurity content of less than 1 wt %, preferably the metal oxide content in the silicon nitride powder is less than 1 wt %, and the sintered body has a thermal conductivity of 90 W / mK or more and a bending strength of 700 MPa or more, and preferably the sintering conditions for the sintered body are as follows: the silicon nitride powder is mixed with MgO, Y 2 O 3 The powder is mixed with the above powder, polished, and the powder is dry-press molded, and the powder is gas-pressure sintered at 1900°C and a nitrogen gas pressure of 1 MPa for 8 hours.

[0005] Patent Document 3 discloses a silicon nitride powder suitable for producing a highly thermally conductive silicon nitride sintered body. The silicon nitride powder is characterized by having a β fraction of 30 to 100%, an oxygen content of less than 0.5 wt%, an average particle size of 0.2 to 10 μm, an aspect ratio of 10 or less, and containing columnar particles with grooves formed in the long axis direction of the particle.

[0006] JP 2022-522814 A JP 2022-541208 A JP 2004-262756 A

[0007] In recent years, the miniaturization of electronic devices and the increasing integration of ICs have narrowed the gap between electronic components and heat sinks. Resin compositions placed between electronic components and heat sinks are required to be moldable into such narrow gaps (i.e., have excellent moldability). Furthermore, after molding, the resin composition is required to conform to the gap without spilling out (this shape stability of the resin composition after molding is referred to as "curability" in this specification). If the resin composition cannot maintain its shape after molding into the gap until curing is complete, it may spill out and adversely affect surrounding electronic components, etc., which is undesirable. Therefore, a resin composition that can maintain its shape after molding (i.e., has excellent curability) is desired. To achieve both excellent moldability and excellent curability, it is effective to increase the shear rate dependence of the viscosity of the resin composition (a mixture of resin and silicon nitride powder) before curing. Therefore, a silicon nitride powder that can increase the shear rate dependence of the viscosity of the mixture is desired.

[0008] However, Patent Documents 1 to 3 do not consider the shear rate dependency of the viscosity of the mixture. For example, Patent Document 1 considers maintaining the viscosity of the mixture low in order to improve the moldability of the resin composition, but does not consider controlling the shear rate dependency of the viscosity of the mixture. Patent Documents 2 and 3 do not consider either the moldability of the resin composition or the control of the shear rate dependency of the viscosity of the mixture.

[0009] In view of these circumstances, one embodiment of the present invention aims to provide a silicon nitride powder for use as a filler for resin compositions, which is capable of increasing the shear rate dependency of the viscosity of a mixture with a resin. Furthermore, another embodiment of the present invention aims to provide a resin composition using the silicon nitride powder.

[0010] A first aspect of the present invention is a silicon nitride powder containing a plurality of silicon nitride particles, wherein, for each silicon nitride particle, a line is drawn passing through a point on the outer shape in a planar view and extending to the left and right of the point, the line having a coefficient of determination R2 of more than 0.98 and not more than 1.00, and the angle formed by the lines in the left and right direction is defined as θ, and the smallest angle θ for each silicon nitride particle is defined as minimum angle θ. min The minimum angle θ min The average value of θ ave-min is less than 106.2°.

[0011] Aspect 2 of the present invention is characterized in that, in the plurality of silicon nitride particles, the minimum angle θ min The silicon nitride powder according to aspect 1, wherein the minimum value of is less than 79.3°.

[0012] A third aspect of the present invention is the silicon nitride powder according to the first or second aspect, wherein the ratio (D90 / D50) of the particle diameter D90 at 90% cumulative particle size from the fine side of the volume-based cumulative particle size distribution to the particle diameter D50 at 50% cumulative particle size from the fine side of the volume-based cumulative particle size distribution is less than 4.8.

[0013] A fourth aspect of the present invention is the silicon nitride powder according to any one of the first to third aspects, wherein the silicon nitride particles have an average aspect ratio of the minor axis to the major axis of less than 0.87.

[0014] A fifth aspect of the present invention is the silicon nitride powder according to any one of the first to fourth aspects, wherein the ratio (L2 / L1) of the total length L2 of the internal boundary lines to the length L1 of the outer edge is 1% or less, and the maximum particle size of the silicon nitride particles is 6.8 μm or more.

[0015] A sixth aspect of the present invention is a resin composition comprising a resin and the silicon nitride powder according to any one of the first to fifth aspects.

[0016] When the silicon nitride powder according to one embodiment of the present invention is mixed with a resin, the viscosity of the mixture is highly dependent on shear rate. This results in excellent moldability and curability during molding. A resin composition according to another embodiment of the present invention uses the silicon nitride powder according to one embodiment, and therefore the viscosity of the mixture is highly dependent on shear rate. This results in excellent moldability and curability during molding.

[0017] The minimum angle θ of silicon nitride particles contained in silicon nitride powder min 1 is a schematic diagram for explaining a method for determining the angle θ by drawing a straight line on a silicon nitride particle contained in a silicon nitride powder.

[0018] [Silicon Nitride Powder] In order to achieve both excellent moldability and curability during molding, the inventors investigated the viscosity of a mixture (a resin composition before curing) of a resin and silicon nitride powder as a filler from various perspectives. They found that these two properties can be achieved if the viscosity of the mixture is highly shear-rate dependent (specifically, has shear-thinning properties). By reducing the viscosity of the mixture at high shear rates, the mixture can be poured into narrow gaps, thereby achieving excellent moldability. On the other hand, by increasing the viscosity of the mixture at low shear rates, the mixture can retain its shape after pouring into narrow gaps, and when cured, a resin composition (after curing) that does not overflow from the gaps can be obtained. This allows the resin composition to achieve excellent curability during molding.

[0019] As a result of further intensive research, the inventors discovered for the first time that controlling the shape of silicon nitride particles is important for achieving shear rate dependency of the viscosity of a mixture, and that it is particularly important that the silicon nitride particles have angular portions in a planar view, leading to the completion of the present invention. The silicon nitride powder according to an embodiment of the present invention is intended to be used as a filler for a resin composition by mixing it with a resin. The silicon nitride powder is prepared by drawing lines passing through a point on the outer shape in a planar view and to the left and right of the point, with a coefficient of determination R2 of more than 0.98 and not more than 1.00, and the angle formed by the lines in the left and right directions is defined as θ, and the smallest angle θ for each silicon nitride particle is defined as the minimum angle θ. min and the minimum angle θ min The average value of θ ave-min The shear rate dependency of viscosity of the resin composition (a mixture of resin and silicon nitride powder) before curing can be increased by having this characteristic. Each of the characteristics will be described below.

[0020] (Minimum angle θ of silicon nitride particles min The average value of θ ave-min The silicon nitride powder of this embodiment contains a plurality of silicon nitride particles. The silicon nitride powder has a minimum angle θ min The average value of θ ave-min The minimum angle θ is less than 106.2°. min The average value of θ ave-min The method for calculating " is explained in detail below.

[0021] FIG. 1 is a schematic diagram of a single silicon nitride particle 10 when viewed in plan. Point p is placed at an arbitrary position on the outline (sometimes referred to as the "outline") 10L of the silicon nitride particle 10 in plan view. The outline (outline) in plan view refers to a shape that appears in a two-dimensional image, such as a scanning electron microscope image (SEM image), that can be obtained, for example. Next, two straight lines L1 and L2 passing through point p are drawn, one on each side of point p (for convenience, referred to as the "left and right directions of point p"). In this case, lines L1 and L2 are drawn so that the coefficient of determination R2 is greater than 0.98 and less than 1.00 with respect to the outline (outline) 10L extending to the left and right of point p. A specific method for drawing the lines will be explained with reference to FIG. 2. In FIG. 2, three points p are deliberately drawn within a range of the outline 10L of the silicon nitride particle 10 that would not be recognized as a "straight line with a coefficient of determination R2 greater than 0.98 and less than 1.00." 1 ~p 3 Please note that the following is set.

[0022] On the contour line 10L of the silicon nitride particle 10, three arbitrary points p 1 ~p 3 (See Figure 2). If all of the conditions (i) to (iii) described below are satisfied, the three points p 1 ~p 3 The points p on both ends of 1 , p 3 In this embodiment, the line L1 (a line extending from point p to the right) is the line L2 having a coefficient of determination R2 of more than 0.98 and not more than 1.00. 1 The remaining two points are 2 , p 3When drawing a line L2 (a line extending leftward from point p), point p in FIG. 1 is set to point p in FIG. 3 The remaining two points are 2 , p 2 Set.

[0023] Condition (i) 3 points p 1 ~p 3 The (x, y) coordinates of the three points p are specified, and the coefficient of determination R2 calculated from these coordinates is greater than 0.98 and less than 1. 1 ~p 3 A line connecting any two points (point p 1 and point p 2 A line connecting point p 1 and point p 3 The line connecting the points p 2 and point p 3 The longest line segment defined by the two points (in Figure 1, point p 1 and point p 3 Line segment p 1 p 3 ) length a is 2 μm or more Condition (iii) The two points at both ends of the longest line segment (point p 1 and point p 3 ) the length of the contour line 10L between the two points is b, 1 p 3 The relationship between the length a and the length b satisfies the following formula (1): 1≦b / a<1.01 (1)

[0024] The "coefficient of determination R2" is calculated by the following formula (2), and is calculated by squaring the correlation coefficient.

[0025] Here, x is the average value of xi (i=1-n), and y is the average value of yi (i=1-n).

[0026] The angle formed by the two straight lines L1 and L2 thus drawn (angle θ in FIG. 1) is measured using an angle measurement function of image analysis software (for example, the Angle Tool of Image J (manufactured by the National Institute of Health)).

[0027] The angle θ is measured at multiple points on the outline 10L of each silicon nitride particle 10 in plan view. In particular, it is efficient to visually set a point p on a sharp portion of the outline in plan view and measure the angle θ. The smallest angle among the multiple angles θ is referred to as the "minimum angle θ". min Then, 20 silicon nitride particles are selected from the plurality of silicon nitride particles present in the planar image (for example, SEM image), and the minimum angle θ min Determine the minimum angle θ min The arithmetic mean value of the minimum angle θ of the silicon nitride powder is calculated. min The average value of θ ave-min Let's say.

[0028] The silicon nitride powder according to this embodiment has a minimum angle θ min The average value of θ ave-min By making the angle θ less than 106.2°, the shear rate dependency of the viscosity of the mixture with the resin can be increased. The reason why such an effect is exhibited is not clear, but it is presumed as follows. ave-min A shear angle of less than 106.2° indicates the presence of angular portions in the silicon nitride particles. At high shear rates, the angular portions of the silicon nitride particles are oriented in the same direction (i.e., the silicon nitride particles are oriented), which is thought to suppress collisions and aggregation between the silicon nitride particles and reduce viscosity. On the other hand, at low shear rates, the angular portions of the silicon nitride particles are not oriented, which is thought to make collisions and aggregation between the silicon nitride particles more likely to occur, resulting in an increase in viscosity.

[0029] In fact, it has been confirmed that the mixture of silicon nitride powder and resin according to the embodiment has shear-thinning properties (low viscosity at high shear rates and high viscosity at low shear rates). Molding a resin composition from a shear-thinning mixture results in excellent moldability and excellent curing properties during molding.

[0030] Silicon nitride powder has a minimum angle θ min The average value of θ ave-minis preferably 106.10° or less, more preferably 100.0° or less, even more preferably 97.0° or less, still more preferably 95.0° or less, still more preferably 93.0° or less, and particularly preferably 90.0° or less. min The average value of θ ave-min is, for example, 60.0° or more, 70.0° or more, or 77.0° or more.

[0031] (Minimum angle θ min The minimum value of the minimum angle θ min The minimum value of the minimum angle θ is preferably less than 79.3°, more preferably 79.0° or less, even more preferably 75.0° or less, still more preferably less than 68.9°, even more preferably 66.0° or less, and particularly preferably 60.0° or less. This increases the shear rate dependency of the viscosity of the mixture of silicon nitride powder and resin, thereby further improving moldability and hardening during molding. min The minimum value of is, for example, 30.0° or more, 42.0° or more, or 44.0° or more.

[0032] minimum angle θ min The method for measuring the minimum angle θ is the same as that described above. Then, 100 silicon nitride particles present in a planar image (for example, an SEM image) are selected, and the minimum angle θ of each of the 100 silicon nitride particles is measured. min Determine the minimum angle θ min Find the smallest value among these and calculate the minimum angle θ min The minimum value of

[0033] (D90 / D50) (D50 is the cumulative 50% particle diameter from the fine side of the cumulative particle size distribution on a volume basis, and the ratio of D90 is the cumulative 90% particle diameter from the fine side of the cumulative particle size distribution on a volume basis to D50) The silicon nitride powder preferably has a cumulative 50% particle diameter D50 from the fine side of the cumulative particle size distribution on a volume basis (hereinafter simply referred to as "D50") of 1.5 μm or more, more preferably 2.0 μm or more. There is no particular upper limit, but for example, it is preferably 500 μm or less, more preferably 300 μm or less, and even more preferably 200 μm or less.

[0034] If the particle size distribution of the silicon nitride powder is sharp on the large particle size side, the viscosity of the mixture of the silicon nitride powder and the resin will be highly dependent on shear rate, which will further improve moldability and curability during molding. Therefore, for example, D90 / D50 is preferably less than 4.8, more preferably 4.6 or less, even more preferably less than 4.0, even more preferably 3.5 or less, and particularly preferably 3.0 or less. There is no particular restriction on the lower limit of D90 / D50, but from the viewpoint of production stability, it is preferably greater than 1.2.

[0035] The D90 and D50 of silicon nitride powder are measured by laser diffraction. Specifically, the powder is dispersed in water and irradiated with a laser beam, and the diffraction is measured to determine each particle size. A measuring device such as the 1090L manufactured by CILAS can be used.

[0036] (Average aspect ratio of silicon nitride particles) The average aspect ratio of the minor axis to the major axis of the silicon nitride particles contained in the silicon nitride powder is preferably greater than 0.50, more preferably greater than 0.60, and even more preferably 0.67. On the other hand, the average aspect ratio of the silicon nitride particles is preferably less than 0.87, more preferably 0.85 or less. When the average aspect ratio of the silicon nitride particles is within an appropriate range, the viscosity of the mixture of the silicon nitride powder and the resin is highly dependent on the shear rate, which can further improve moldability and the effect of suppressing burrs during molding.

[0037] The average aspect ratio of silicon nitride particles is measured as follows. SEM images of silicon nitride particles contained in silicon nitride powder are analyzed using image processing software (e.g., Image J (manufactured by the National Institute of Health)). The maximum particle size of the silicon nitride particles (referred to as the "major axis") is identified, and the particle size in the direction perpendicular to the major axis is referred to as the "minor axis". The major and minor axes are measured for 20 random silicon nitride particles, and the ratio of the minor axis to the major axis (minor axis / major axis) is determined for each particle. The arithmetic mean value of these ratios is taken as the average aspect ratio of the silicon nitride particles.

[0038] (The maximum particle size of silicon nitride particles having a ratio (L2 / L1) of the total length L2 of the internal boundaries to the outer edge length L1 of 1% or less is 6.8 μm or more.) Therefore, the ratio (L2 / L1) of the total length L2 of the boundaries to the outer edge length L1 is introduced as an index of the content of grain boundaries within silicon nitride particles. L1 and L2 are determined by observing the cross section of the silicon nitride particle. Note that the terms "grain boundary" and "boundary line" used here refer to boundaries where the crystal orientation misorientation (oblique angle) exceeds 15° as a result of EBSD analysis (also called high-angle grain boundaries).

[0039] When the length of the outer edge of one silicon nitride particle is L1 and the total length of the boundary lines of that silicon nitride particle is L2, silicon nitride particles with a small value of L2 / L1 can be said to have a low content of boundary lines. In this embodiment, silicon nitride particles with an L2 / L1 ratio of 1% or less are considered to be silicon nitride particles consisting of a single crystal (these are referred to as "single crystal particles").

[0040] In this embodiment, the maximum particle size of silicon nitride particles having an L2 / L1 ratio of 1% or less (i.e., single crystal) is preferably 6.8 μm or more, more preferably 10.0 μm or more, and even more preferably 15.0 μm or more. When such silicon nitride particles are mixed with a resin, they can increase the shear rate dependency of the viscosity of the mixture.

[0041] (β-phase ratio) The β-phase ratio of the silicon nitride powder is preferably 65% ​​or more, more preferably 70% or more, even more preferably 80% or more, still more preferably 85% or more, and particularly preferably 90% or more.

[0042] In this specification, the "β-phase ratio" refers to the content (volume %) of β-type silicon nitride relative to all silicon nitrides contained in the silicon nitride powder.

[0043] In calculating the β-phase ratio, the silicon nitride powder was measured by powder X-ray diffraction, and the diffraction pattern was analyzed by the Gazzara & Messier method (G.P. Gazzara and D.P. Messier, "Determination of Phase Content of Si 3 N 4 The β-phase ratio is calculated by analyzing the β-phase by X-ray Diffraction Analysis, Am. Ceram. Soc. Bull., 56[9]777-80 (1977)).

[0044] [Method for Producing Silicon Nitride Powder] A method for producing silicon nitride powder according to an embodiment of the present invention will be described. The method for producing silicon nitride powder includes the steps of: (1) synthesizing silicon nitride synthetic crystals by combustion synthesis in a nitrogen atmosphere using raw materials containing Si; (2) crushing the silicon nitride synthetic crystals to obtain coarsely pulverized silicon nitride powder; and (3) finely pulverizing the coarsely pulverized silicon nitride powder to obtain finely pulverized silicon nitride powder. Optionally, the method may further include the step of: (4) heat-treating the finely pulverized silicon nitride powder.

[0045] Step (1): Synthesizing silicon nitride composite crystals. For example, Si powder is used as the raw material containing Si. The average particle diameter D50 of the raw material is, for example, within the range of 2 to 10 μm. This allows the amount of oxygen impurities to be suppressed, and the combustion rate to be increased, allowing for a higher synthesis temperature, resulting in good crystal growth. As an example, the average particle diameter D50 of Si is 5 μm.

[0046] The diluent is used to adjust the amount of Si in the raw materials. Separately prepared silicon nitride powder is used as the diluent. The diluent may be either α-type silicon nitride powder or β-type silicon nitride powder, or a mixture of these. The average particle diameter D50 of the diluent is preferably in the range of 0.5 to 2.0 μm. As an example, the average particle diameter D50 of the diluent is 1.0 μm. The amount of diluent added is less than 10 mass % of the total raw materials (including the diluent). As an example, the diluent is added in an amount of 5 to 8 mass % of the total raw materials. When the amount of diluent added is within the above range, the minimum angle θ min The average value of θ ave-min A predetermined amount of silicon nitride particles having a predetermined value can be produced.

[0047] In this embodiment, a diluent is mixed with the raw materials and then filled into an insulated heat-resistant container. This insulated heat-resistant container has a thermal conductivity of 1 W / mK or less, and although alumina or zirconia can be used as the material, carbon is preferred to prevent impurities from being mixed in. After the raw materials are filled, the container is covered with a lid made of the same material as the insulated heat-resistant container. Furthermore, to increase the temperature inside the composite during combustion, the thickness of the mixed raw materials is set to more than 100 mm, preferably more than 100 mm and 150 mm or less. Combustion synthesis is performed in a nitrogen atmosphere in the range of 0.5 to 1 MPa (e.g., 0.9 MPa). Adjusting the pressure range within this range enables efficient synthesis while suppressing increases in equipment costs.

[0048] When the mixed raw material is filled into the crucible, a layer of powder (silicon nitride) having a thickness of 1 mm to 80 mm is laid on the bottom and sides of the crucible, and then the mixed raw material is filled. The top surface is then covered with a layer of powder having a thickness of 1 mm to 80 mm. By covering the entire surface with the powder, the mixed raw material can be kept warm, and the minimum angle θ min The average value of θ ave-min A predetermined amount of silicon nitride particles having a predetermined value can be produced.

[0049] To promote crystal growth more effectively, a catalyst may be used, for example, Y 2 O 3 , Fe 2 O 3, CaO, Ni, Co, C, etc. are added in an amount of about 0.01 to 0.1 mass %. In addition, external auxiliary heating is performed in the range of 500°C to 1700°C (for example, 1500°C), and the combustion temperature is also increased in the combustion synthesis method by self-ignition.

[0050] Step (2): Obtaining a coarsely pulverized silicon nitride powder. The silicon nitride composite crystal is in the form of an agglomeration of multiple silicon nitride particles. In step (2), the silicon nitride composite crystal is crushed to obtain a coarsely pulverized silicon nitride powder. For example, the composite is crushed using a common crushing device such as a hammer mill or a disk mill until it passes through a sieve with a specified mesh size (for example, a sieve with mesh sizes in the range of 400 μm to 500 μm).

[0051] Step (3): Step of Obtaining Finely Pulverized Silicon Nitride Powder The coarsely pulverized silicon nitride powder is further pulverized to obtain a finely pulverized silicon nitride powder. The pulverization is carried out using a pulverizing device such as a jet mill or a ball mill. If necessary, the resulting finely pulverized powder may be classified. Classification may be carried out by sieving, wet classification, or the like. The resulting finely pulverized powder may be used as is as the silicon nitride powder, or may be subjected to a heat treatment step (step (4) described below) before use as the silicon nitride powder.

[0052] Step (4): Heat-treating the finely pulverized silicon nitride powder. Optionally, the finely pulverized silicon nitride powder may be heat-treated. Heat treatment forms an oxide film on the surface of the silicon nitride particles, which has the effect of chemically stabilizing the silicon nitride particles. The heat treatment is carried out, for example, in air at a temperature of 500°C or higher and 1200°C or lower. The heat treatment time can be adjusted appropriately according to the heat treatment temperature. The heat treatment time is, for example, 5 hours.

[0053] In the method for producing silicon nitride powder, silicon nitride synthetic crystals are synthesized using the heat generated by combustion synthesis, and then the silicon nitride powder according to this embodiment can be produced by crushing, classifying, and pulverizing the synthesized crystals.

[0054] [Resin composition] The silicon nitride powder according to the embodiment of the present invention is suitable as a filler for a resin composition because it can increase the shear rate dependency of the viscosity of a mixture with a resin. The resin composition contains a resin and the silicon nitride powder according to the embodiment of the present invention. By using the silicon nitride powder according to the embodiment as a filler for a resin composition, the shear rate dependency of the viscosity of the mixture (resin composition before curing) can be increased when mixed with a resin. As a result, a resin composition that can achieve both excellent moldability and excellent curability can be obtained.

[0055] The compounding ratio of the silicon nitride powder to the resin according to the embodiment of the present invention can be determined appropriately depending on the purpose and application. As an example, the resin may be 5 to 75 volume % and the silicon nitride powder may be 95 to 25 volume % relative to the resin composition (composite). The filling rate of the silicon nitride powder in the resin composition refers to the content (vol %) of the silicon nitride powder when the volume of the resin composition (including the silicon nitride powder) is taken as 100 volume %.

[0056] A method for producing a resin composition will be described. A resin composition can be obtained by mixing silicon nitride powder and a resin using a commonly used known method. For example, when the resin is liquid (e.g., liquid epoxy resin), the resin composition can be obtained by mixing the liquid resin, silicon nitride powder, and a curing agent, and then curing the mixture with heat or ultraviolet light. Known curing agents, mixing methods, and curing methods can be used. On the other hand, when the resin is solid, the desired resin composition can be obtained by mixing the silicon nitride powder and the resin, and then kneading the mixture using a known method such as melt kneading.

[0057] The resin used in the resin composition can be a known resin such as an epoxy resin. The type of resin can be selected from thermoplastic resins, thermoplastic elastomers, and thermosetting resins. The resins can be used alone or in combination of two or more.

[0058] Furthermore, these resin compositions may contain, as needed, known additives such as plasticizers, curing accelerators, coupling agents, fillers, pigments, flame retardants, antioxidants, surfactants, compatibilizers, weather resistance agents, antiblocking agents, antistatic agents, leveling agents, and release agents, either singly or in combination, within the scope of the invention.

[0059] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples carried out to clarify the effects of the embodiments of the present invention. However, the embodiments of the present invention are not limited to the following examples.

[0060] <Silicon Nitride Powder Preparation> (Samples No. 1-3) Si powder (particle size = 5 μm) and silicon nitride powder (particle size = 1 μm) prepared separately as a diluent were mixed in a tumbling ball mill. The amount of diluent added was 5-8 mass% of the total raw material (including diluent). The mixed powder was packed into a carbonaceous, heat-resistant container with a 1-80 mm thick layer of powder on the bottom and sides, so that the raw material layer was thicker than 100 mm and not more than 150 mm. The raw material layer was further covered with a 1-80 mm thick layer of powder, and then a lid made of a carbonaceous, heat-resistant material was placed over the container. Synthesis was carried out under a nitrogen atmosphere at 0.9 MPa. After synthesis, the mixture was coarsely crushed (disintegrated) in a mortar until it passed through a sieve with the specified mesh size. The mesh size of the sieve for each sample is shown in Table 1.

[0061] The obtained coarsely pulverized powder was further finely pulverized using a nanojetmizer (manufactured by Aisin Nano Technologies Co., Ltd.). A nanojetmizer with the model number listed in Table 1 was used for the fine pulverization. The obtained finely pulverized powder was classified using the method listed in Table 1. Note that classification was not performed for Sample No. 2. The obtained classified powders (Samples No. 1 and No. 3) and finely pulverized powder (Sample No. 2) were then placed in an alumina crucible and heat-treated in an air atmosphere using a small powder programmable electric furnace (MMF series, manufactured by AS ONE) under the conditions (heat treatment temperature, heat treatment time) listed in Table 1 to obtain silicon nitride powders (Samples Nos. 1 to 3).

[0062] (Samples No. 5 and 6) Coarsely pulverized powders were prepared in the same manner as in Samples No. 1 to 3 above. The sieve used for coarse pulverization (disintegration) had a mesh size of 500 μm. The obtained coarsely pulverized powder was then finely pulverized in a ball mill. The obtained finely pulverized powder was sieved using a vibrating sieve according to the following procedure, and then further wet-classified to obtain silicon nitride powders (Samples No. 5 and 6) having the desired D50. - Sample No. 5: Silicon nitride particles remaining on the sieve after sieving using a sieve with a mesh size of 150 μm (D50: 192.0 μm). - Sample No. 6: Powder remaining on the sieve after sieving using a sieve with a mesh size of 106 μm was further sieved using a sieve with a mesh size of 75 μm, and the silicon nitride particles remaining on the sieve (D50: 83.0 μm).

[0063]

[0064] Various measurements were performed on the obtained Samples Nos. 1 to 3, and 5 and 6 (Examples), and on a commercially available silicon nitride powder (manufactured by Aldrich, silicon nitride (predominantly β-phase, ≦10 micron primary particle size, product code 248622); hereinafter referred to as "Sample No. 4") as a comparative example.

[0065] (1) Measurement of the β-phase ratio of silicon nitride powder A diffraction pattern of the sample (silicon nitride powder) was obtained using a powder X-ray diffractometer (manufactured by Rigaku Denki). The measurement conditions were as follows: X-ray source: CuKα radiation X-ray output: 45 kV, 200 mA Graphite monochromator Diffraction angle (2θ): Step scan in 0.02° increments over the range of 2 to 90° Scanning speed: 21.7 deg / min

[0066] When a sample contained components other than silicon nitride, the peaks of those components were compared with the corresponding peaks of standard samples of those components to determine the proportions of those components. For Samples No. 1 to 6, the powder X-ray diffraction patterns obtained confirmed that the samples were composed solely of α-type silicon nitride and β-type silicon nitride. The proportion of β-type silicon nitride in the sample (β-conversion ratio) was then calculated using the Gazzara & Messier method.

[0067] (2) Maximum particle size of silicon nitride particles with an L2 / L1 ratio of 1% or less (maximum particle size of single-crystal particles) A ​​sample for cross-sectional observation was prepared using the sample (silicon nitride particles). To prepare the sample for cross-sectional observation, the silicon nitride particles were embedded in resin, and then the resin and silicon nitride particles were cut using a diamond cutter. Subsequently, a protective film of platinum was vapor-deposited on the cross-section, and the cross-section was prepared by Ar ion milling. The sample was then fixed to the SEM sample stage with Cu double-sided tape, and SEM-EBSD measurement was performed without vapor deposition. The observation position was determined so that two or more silicon nitride particles were completely contained within the observation region (i.e., two or more silicon nitride particles did not come into contact with the frame of the observation region). Measurements were performed using β-type silicon nitride particles.

[0068] The following equipment was used for sample pretreatment and EBSD measurement: Equipment used Ion milling equipment: E-3500 (manufactured by Hitachi High-Tech Corporation) Ion sputtering equipment: E-1030 (manufactured by Hitachi, Ltd.) Schottky scanning electron microscope: SU5000 (manufactured by Hitachi High-Tech Corporation) Backscattered electron diffraction equipment: Velocity (manufactured by METEK Corporation)

[0069] The conditions for the EBSD measurement were as follows: Measurement area: 500.0 μm×400.0 μm Acceleration voltage: 15.0 kV Magnification: ×500 Vacuum degree: 30 Pa

[0070] In the obtained EBSD image, two or more silicon nitride particles that were not in contact with the frame of the observation area were selected, and the average of the outer edge length L1 of each silicon nitride particle was calculated using image processing software Image J (manufactured by the National Institute of Health). The total length L2 of the boundary lines was also calculated. The "total length L2 of the boundary lines" is the sum of the boundary lines contained within the silicon nitride particle and does not include the outer edge of the silicon nitride particle. The total length L2 of the boundary lines was calculated by adding the total length of the grain boundaries within the silicon nitride particle and the total length of the inner walls of the cavities (if any) within the silicon nitride particle.

[0071] This measurement was carried out once for 20 random silicon nitride particles, and silicon nitride particles with an L2 / L1 ratio of 1% or less were considered to be single crystal particles, and the length of their major axis was measured and recorded as the "maximum particle size of the single crystal particles." If the 20 silicon nitride particles measured contained multiple single crystal particles, the arithmetic average of their maximum particle sizes was calculated.

[0072] (3) Calculation of (D90 / D50) of silicon nitride powder The particle size distribution of the sample (silicon nitride powder) was measured, and the cumulative 90% particle size D90 and cumulative 50% particle size D50 were determined, and (D90 / D50) was calculated using these. The particle size distribution of the silicon nitride powder was measured by laser diffraction. A sample dispersed in water was irradiated with a laser beam, and the diffraction was measured to determine the particle size. The measuring device used was a CILAS 1090L model. The particle size was taken as the circle-equivalent particle size. The circle-equivalent particle size is the particle size of a perfect circle that has the same area as a projected particle image. The particle size was measured by volume.

[0073] (4) Average aspect ratio of silicon nitride particles SEM images of the sample (silicon nitride powder) were taken. The following equipment was used for taking the images. Equipment used: Scanning electron microscope: JSM-IT200 (manufactured by JEOL Ltd.) The imaging conditions were as follows: Acceleration voltage: 5.0 kV Signal: SED Probe current: Std. -PC55 Magnification: 1000x

[0074] The SEM images were processed using image processing software Image J (manufactured by the National Institute of Health), and the aspect ratios of 20 randomly selected silicon nitride particles in the SEM images were determined. The maximum diameter of the silicon nitride particles was taken as the major axis, and the particle size in the direction perpendicular to the major axis was taken as the minor axis. The major and minor axes of 20 randomly selected silicon nitride particles were measured, and the ratio of the minor axis to the major axis (minor axis / major axis) was determined for each particle. The arithmetic mean value of these ratios was taken as the average aspect ratio of the silicon nitride particles (referred to as "aspect ratio" in the table).

[0075] (5) Minimum angle θ min Measurement of the minimum angle θ for each of 100 arbitrary silicon nitride particles by image analysis of the SEM image acquired in "(4) Average aspect ratio of silicon nitride particles"min The minimum angle θ min was determined using the method shown in FIG. 1 and described above. The minimum angle θ obtained min 20 data are arbitrarily selected from the data (100 data), and their arithmetic mean value is calculated as the minimum angle θ min The average value of θ ave-min The minimum angle θ min The smallest value (minimum value) was determined from the data (100 data).

[0076] (6) Viscosity Measurement of Resin and Silicon Nitride Powder Mixtures Shear rate-viscosity measurements were performed on mixtures of the sample silicon nitride powder with epoxy resin. Epoxy resin (Mitsubishi Chemical's epoxy binder jER828) and one of the silicon nitride powders No. 1 to 6 were mixed at a volume ratio of 60:40 (equivalent to approximately 1.5 g of epoxy resin and approximately 3.0 g of silicon nitride powder). The silicon nitride powder and epoxy resin were manually mixed in a mortar for approximately 10 to 20 minutes to prepare a mixed sample for viscosity measurement.

[0077] The shear rate-viscosity of the mixed sample was measured using a HAAKEMARSID (manufactured by Thermo Fisher Scientific). The measurement conditions were as follows: Geometry: Φ20 mm parallel plate Shear rate: 1 s -1 ~1000s -1 Measurement temperature: 23°C Measurement time: 4 minutes The sample was set on the plate stabilized at the measurement temperature within 10 minutes, and measurement was started.

[0078] Shear rate 1 s -1 Viscosity η 1 and 563s -1 Viscosity η at 563 were calculated. -1 Viscosity η at 563 For 1s -1 Viscosity η 1 The ratio (η 1 / η 563 ) was calculated to evaluate the shear rate dependency of viscosity.

[0079] (7) Moldability of resin composition (composite) An epoxy resin (main agent: room temperature curing potting resin 53 type (manufactured by Sankei Co., Ltd.) 010-8140, curing agent: room temperature curing potting resin 53 type (manufactured by Sankei Co., Ltd.) 010-8143) and a sample (silicon nitride powder) were mixed in a blending ratio (volume ratio) of 50:50, and the mixture was stirred and mixed using a Foam Mixer (manufactured by Thinky Corporation) to obtain an epoxy resin-filler (silicon nitride powder) composite. The filling rate of the silicon nitride powder in the resin composition was 50% by volume.

[0080] (Test method for evaluating moldability and curability) A mold was prepared by drilling a rectangular hole measuring 1 cm x 10 cm in a 1 mm thick aluminum plate. A transparent PET film (back side film) coated with a release agent was attached to the back side of the mold so as to cover the rectangular hole in the mold, with the surface coated with the release agent facing the mold. 1 g of the resin composition (gray) was poured into the rectangular hole in the mold, and then a transparent PET film (front side film) coated with a release agent was attached on top of it, with the surface coated with the release agent facing the mold and the resin composition. Furthermore, a metal roller was lightly pressed from above the front side film to fit the resin composition into the rectangular hole in the mold and molded into a 1 cm x 10 cm strip. The roller was then removed, and the resin composition was allowed to stand for 5 minutes. The state of the resin composition (gray) was observed through the backside film to check (1) whether the entire rectangular hole in the mold was filled with the resin composition without any defects (e.g., voids) (confirmation of moldability), and (2) whether the resin composition protruded outside the rectangular hole in the mold (confirmation of curability). Regarding (1), if there were no defects (voids) with a maximum dimension of 1 mm or more, the result was deemed "pass." Regarding (2), the mold was observed from the backside, the position of the rectangular hole was identified, and if the resin composition protruded less than 1 mm from each side of the rectangular hole, the result was deemed "pass." If both (1) moldability and (2) curability were passed, a "good" was entered in the "Moldability and Curability" column in Table 3. If either or both were unsuccessful, a "bad" was entered.

[0081] The measurement results are summarized in Tables 2 and 3.

[0082]

[0083]

[0084] The measurement results are discussed below. Composites (before curing) using silicon nitride powders of Samples Nos. 1 to 3 and 5 and 6, which satisfied the requirements of this embodiment, had high shear rate dependency of viscosity. Therefore, they had good moldability and curability. On the other hand, the composite using silicon nitride powder of Sample No. 4, which did not satisfy the requirements of this embodiment, had poor moldability and curability.

[0085] This application claims priority from Japanese Patent Application No. 2023-058747, filed March 31, 2023. Japanese Patent Application No. 2023-058747 is incorporated herein by reference.

Claims

1. A silicon nitride powder containing a plurality of silicon nitride particles, wherein, for each silicon nitride particle, a straight line is drawn passing through a point on the outer shape in a planar view and in the left-right direction of the point, with a coefficient of determination R2 of more than 0.98 and not more than 1.00, and the angle formed by the straight lines in the left-right direction is defined as θ, and the smallest angle θ for each silicon nitride particle is defined as the minimum angle θ min The minimum angle θ min The average value of θ ave-min A silicon nitride powder having a refractive index of less than 106.2°.

2. In the plurality of silicon nitride particles, the minimum angle θ min The silicon nitride powder according to claim 1, wherein the minimum value of is less than 79.3°.

3. The silicon nitride powder according to claim 1, wherein the ratio (D90 / D50) of the particle diameter D90 at the cumulative 90% from the fine side of the volume-based cumulative particle size distribution to the particle diameter D50 at the cumulative 50% from the fine side of the volume-based cumulative particle size distribution is less than 4.

8.

4. The silicon nitride powder according to claim 1, wherein the silicon nitride particles have an average aspect ratio of the minor axis to the major axis of less than 0.

87.

5. The silicon nitride powder according to claim 1, wherein the maximum particle size of silicon nitride particles having a ratio (L2 / L1) of the total length L2 of the internal boundary lines to the length L1 of the outer edge of the silicon nitride particles is 6.8 μm or more.

6. A resin composition comprising a resin and the silicon nitride powder according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Method for preparing beta-silicon nitride powder

    CN101857441A

  • Equiaxial beta-Si3N4 powder and preparation process thereof

    CN114477111A

  • Silicon nitride powder and its production

    JP1990248309A

  • Method for manufacturing silicon nitride powder

    WO2019167879A1

  • Columnar particles of β-silicon nitride, composite particles, sintered substrate for heat radiation, resin composite, inorganic composite, method for producing columnar particles of β-silicon nitride, and method for producing composite particles

    WO2023210649A1