Polymer fine particle, method for producing same, composition, optical member, light source unit, display and lighting device, and ink
The production of polymer fine particles with specific resin and luminescent material compositions and structures addresses the challenges of sphericity and durability, achieving enhanced performance and stability in high-illuminance applications by ensuring high sphericity and reduced optical losses.
Patent Information
- Application Number
- PCT/JP2024/006549
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-02-22
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional methods for producing polymer fine particles face limitations in achieving high sphericity, uniformity, and isotropy, leading to optical losses and accelerated deterioration, especially in high-illuminance optical applications, due to irregular particle shapes and residual impurities.
The development of polymer fine particles with a sphericity of 80-100%, containing a resin with ring structures and a luminescent or coloring material, characterized by specific molecular structures and low solvent content, which are produced through a method involving emulsion formation and solvent removal without polymerization, ensuring high purity and reduced optical losses.
The resulting polymer fine particles exhibit improved durability and reduced optical loss, suitable for long-term use in high-illuminance optical applications with enhanced sphericity and uniformity, maintaining performance and stability.
Smart Images

Figure JP2024006549_03102024_PF_FP_ABST
Abstract
Description
Polymer microparticles, method for producing the same, composition, optical member, light source unit, display and lighting device, ink
[0001] The present invention relates to polymer microparticles and a method for producing the same, a composition and optical member containing the polymer microparticles, and a light source unit, a display, a lighting device, and an ink produced using the polymer microparticles.
[0002] Polymer microparticles are fine particles made of polymers, typically ranging in diameter from several tens of nanometers to several hundred micrometers. Unlike polymer molded products such as films, fibers, injection-molded products, and extrusion-molded products, polymer microparticles have a large specific surface area and a fine particle shape, making them suitable for use in modifying and improving various materials. Major applications of polymer microparticles include cosmetic modifiers, toner additives, optical applications such as light diffusion and light absorption, rheology modifiers for paints, medical diagnostic testing agents, additives for molded products such as automotive materials and building materials, and powder raw materials for 3D printers.
[0003] Conventional methods for producing polymer microparticles can be broadly divided into build-up processes, such as radical polymerization, and top-down processes, such as mechanical pulverization and solution precipitation. A typical build-up process is a radical polymerization method of vinyl polymers, such as emulsion polymerization (see, for example, Patent Document 1). Typical top-down processes that are easily used are mechanical pulverization and solution precipitation. Mechanical pulverization involves freezing resin pellets, for example, with liquid nitrogen, and mechanically pulverizing them. Solution precipitation involves dissolving a resin in a solvent, reducing the solubility of the resin by cooling or solvent removal, thereby precipitating the resin into particles to obtain microparticles (see, for example, Patent Document 2).
[0004] Furthermore, polymer microparticles containing luminescent materials and coloring materials have been studied for use as marking materials for biological observation and as optical components. As a method for producing such polymer microparticles, a method of forming particles by spray drying a mixture of a luminescent material and an acrylic resin has been reported (see, for example, Patent Document 3).
[0005] Japanese Patent Application Laid-Open No. 7-133328 Japanese Patent Application Laid-Open No. 2005-054153 International Publication No. 2020 / 050144
[0006] However, the resins considered for the build-up process described in Patent Document 1 are limited to certain vinyl polymers made from raw materials such as acrylic and styrene, which limits the ability to obtain polymer microparticles with the desired resin suitable for optical applications. Furthermore, since the polymers are produced by polymerizing emulsified monomers, it is inevitable that emulsifiers, polymerization initiators, and altered products thereof will remain in the polymer microparticles after polymerization, which poses a problem of changes in optical properties such as coloration caused by trace impurities during long-term use in optical applications.
[0007] On the other hand, the top-down process has the advantage of processing a resin with desired properties into a fine particle shape, thereby obtaining polymer microparticles from a resin with excellent optical performance. Furthermore, since purified, high-purity resin can be directly granulated, it also has the advantage of preventing trace impurities from remaining in the polymer microparticles. However, among these techniques, mechanical pulverization requires freezing the resin, which increases energy costs and has the problem that the resulting pulverized material generally has an irregular shape. Furthermore, even with the dissolution-precipitation method described in Patent Document 2, the resulting microparticles generally have an irregular shape, and the microparticles also have the problem of becoming porous, resulting in a large specific surface area.
[0008] Furthermore, in recent years, the illuminance required for light sources in optical applications has increased, posing a problem of deterioration of components containing luminescent materials or coloring materials. Patent Document 3 discloses a technology for suppressing the propagation of highly active species by microparticulating polymers and suppressing accelerated deterioration of the entire component. However, existing technologies have not yet been able to fully address this issue in light sources with rapidly increasing illuminance. Specifically, design techniques for the composition and shape of polymer microparticles have been insufficient. For example, while the technology disclosed in Patent Document 3 makes it possible to produce polymer microparticles containing luminescent materials or coloring materials, it is insufficient in terms of optimizing the resin that constitutes the polymer microparticles. Furthermore, the irregular shape of the resulting microparticles poses problems of optical loss and accelerated deterioration.
[0009] The problem to be solved by the present invention is to provide polymer microparticles containing a light-emitting material or a coloring material that achieve both improved durability and reduced optical loss. In particular, the present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide polymer microparticles that are made of a resin suitable for long-term use in high-intensity optical applications, and that have high sphericity, excellent uniformity, and isotropy.
[0010] In order to solve the above-mentioned problems and achieve the object, the present invention has the configuration described in any one of [1] to
[25] below.
[0011] That is, the polymer microparticles according to the present invention are characterized in that [1] they are polymer microparticles containing a resin as a main component and containing a light-emitting material or a coloring material, the sphericity being 80 or more and 100 or less, and the resin is a resin having at least one ring structure selected from the group consisting of an aliphatic hydrocarbon ring, an aliphatic heterocycle, and a ring containing an SP3 carbon in its molecular structure.
[0012] The polymer microparticles according to the present invention are characterized in that, in the invention described in [1] above, the polymer microparticles have a linseed oil absorption of 1 mL / 100 g or more and 200 mL / 100 g or less.
[0013] The polymer microparticles according to the present invention are characterized in that, in the invention described in [1] or [2] above, the ratio of the D90 particle size to the D10 particle size in the particle size distribution of the polymer microparticles, D90 particle size / D10 particle size, is 1 or more and 5 or less.
[0014] The polymer microparticles according to the present invention are characterized in that, in the invention described in any one of the above items [1] to [3], the content of the solvent in the polymer microparticles is less than 1 wt %.
[0015] The polymer microparticles according to the present invention are characterized in that, in the invention described in any one of the above items [1] to [4], the content of the polymerization initiator and its decomposition products in the polymer microparticles is less than 0.1 wt %.
[0016] The polymer microparticles according to the present invention are characterized in that, in the invention described in any one of the above items [1] to [5], the glass transition temperature of the resin is 100°C or higher.
[0017] The polymer microparticles according to the present invention are also characterized in that, in the invention described in any one of [1] to [6] above, the resin is at least one of a resin having the ring structure in a polymer main chain and a resin in which the ring structure is directly linked to the polymer main chain.
[0018] The polymer microparticles according to the present invention are also characterized in that, in the invention described in any one of the above items [1] to [7], the resin has a partial structure represented by general formula (1) and a partial structure represented by general formula (2) in its molecular structure.
[0019] (In general formula (1), Y 1 and Y 2 may be the same or different and are a hydrogen atom or an organic group having 1 to 20 carbon atoms. 3 ~Y 6 may be the same or different and each represents a hydrogen atom or an organic group having 1 to 20 carbon atoms, and Y 3 ~Y 6At least one of the groups is a group containing an aliphatic cyclic hydrocarbon structure.
[0020] The polymer particles according to the present invention are also characterized in that, in the invention described in [8] above, Y 3 ~Y 6 At least one of the groups is a substituted or unsubstituted cyclohexyl group.
[0021] The polymer particles according to the present invention may further comprise, in the invention described in [8] above, a polymer having Y of the general formula (2). 3 ~Y 6 is a substituted or unsubstituted cyclohexyl group, and the other three are hydrogen atoms.
[0022] The polymer particles according to the present invention are also characterized in that, in the invention described in any one of the above items [1] to
[10] , the resin has a light transmittance of 85% or more in a wavelength range of 400 nm to 800 nm, and an intrinsic birefringence of −30×10 -4 Above + 30 x 10 -4 The resin is characterized in that it is:
[0023] The polymer particles according to the present invention are characterized in that, in the invention described in any one of the above items [1] to
[11] , the luminescent material or the coloring material is an organic pigment or an organic dye.
[0024] The polymer particles according to the present invention are also
[13] the invention described in any one of [1] to
[12] above, wherein the light-emitting material or the coloring material has a molar absorption coefficient of 10,000 M at a maximum absorption wavelength in a wavelength range of 300 nm or more. -1 ・cm -1 The organic material is characterized by containing at least one of the above organic materials.
[0025] Furthermore, the polymer microparticles according to the present invention are characterized in that, in the invention described in any one of [1] to
[13] above, they contain at least one of the luminescent materials, and the half width of the luminescent spectrum of the luminescent material is 60 nm or less.
[0026] The composition according to the present invention is characterized by containing
[15] a binder resin and the polymer fine particles described in any one of [1] to
[14] above.
[0027]
[16] The optical member according to the present invention is characterized by containing the polymer fine particles according to any one of [1] to
[14] above.
[0028] The light source unit according to the present invention is characterized by comprising:
[17] a light source; and the polymer fine particles according to any one of [1] to
[14] above.
[0029]
[18] A display according to the present invention is characterized by comprising the light source unit according to
[17] above.
[0030]
[19] A lighting device according to the present invention is characterized by comprising the light source unit according to
[17] above.
[0031]
[20] The ink according to the present invention is characterized by containing the polymer fine particles described in any one of [1] to
[14] above.
[0032] The method for producing polymer microparticles according to the present invention is characterized in that it comprises the following steps (a) and (b) carried out in sequence: step (a): forming an emulsion containing two phases: a polymer phase containing a resin having at least one ring structure selected from the group consisting of an aliphatic hydrocarbon ring, an aliphatic heterocycle, and a ring containing SP3 carbon in its molecular structure, and an organic solvent; and a poor solvent phase containing a water-soluble polymer and at least one of water and an alcohol. step (b): subjecting the emulsion to at least one of heating and reducing pressure while stirring to remove part or all of the organic solvent contained in the emulsion, thereby precipitating polymer microparticles.
[0033] The method for producing polymer microparticles according to the present invention is
[22] the method according to the above
[21] , characterized in that the water-soluble polymer is at least one selected from polyvinyl alcohol, poly(vinyl alcohol-ethylene) copolymer, polyethylene glycol, cellulose derivatives, and polyvinylpyrrolidones.
[0034] The method for producing polymer microparticles according to the present invention is
[23] the method according to the above
[21] or
[22] , characterized in that the steps (a) and (b) do not include a polymerization step.
[0035] The method for producing polymer microparticles according to the present invention is characterized in that, in the invention described in any one of
[21] to
[23] above, the resin is at least one of a resin having the ring structure in the polymer main chain and a resin in which the ring structure is directly linked to the polymer main chain.
[0036] The method for producing polymer microparticles according to the present invention is,
[25] , the invention described in any one of
[21] to
[24] above, wherein the resin has a light transmittance of 85% or more in a wavelength range of 400 nm to 800 nm and an intrinsic birefringence of −30×10 -4 Above + 30 x 10 -4 The resin is characterized in that it is:
[0037] The polymer microparticles of the present invention, as well as compositions and optical components containing the same, achieve both improved durability and reduced optical loss, and therefore, by using them, it is possible to obtain light source units, displays and lighting devices, and inks that achieve both improved durability and reduced optical loss.
[0038] Fig. 1 is a scanning electron microscope photograph of polymer microparticles obtained in Example 1. Fig. 2 is a scanning electron microscope photograph of polymer microparticles obtained in Comparative Example 1. Fig. 3 is a scanning electron microscope photograph of polymer microparticles obtained in Comparative Example 2. Fig. 4 is a schematic cross-sectional view showing a first example of an optical member according to an embodiment of the present invention. Fig. 5 is a schematic cross-sectional view showing a second example of an optical member according to an embodiment of the present invention. Fig. 6 is a schematic cross-sectional view showing a third example of an optical member according to an embodiment of the present invention.
[0039] Preferred embodiments of the polymer microparticles, their manufacturing method, composition, optical element, light source unit, display and lighting device, and ink according to the present invention will be specifically described below. However, the present invention is not limited to the following embodiments, and can be modified in various ways depending on the purpose and application.
[0040] In the present invention, "equal to or greater than" means equal to or greater than the indicated numerical value. "equal to or less than" means equal to or less than the indicated numerical value. "less than" means less than the indicated numerical value.
[0041] In all groups of the compounds or partial structures thereof described below, hydrogen may be replaced with deuterium. In the following description, for example, a substituted or unsubstituted aryl group having 6 to 40 carbon atoms refers to an aryl group having 6 to 40 carbon atoms, including the number of carbon atoms contained in the substituents substituted on the aryl group. The same applies to other substituents that specify the number of carbon atoms.
[0042] The term "unsubstituted" in the context of "substituted or unsubstituted" means that a hydrogen atom or a deuterium atom has been substituted. The same applies to the term "substituted or unsubstituted" in the compounds or partial structures thereof described below.
[0043] In all of the groups described below, examples of the substituent when substituted include an alkyl group, a cycloalkyl group, a heterocyclic group, an alkenyl group, a cycloalkenyl group, an alkynyl group, an aryl group, a heteroaryl group, a hydroxyl group, a thiol group, an alkoxy group, an alkylthio group, an aryl ether group, an aryl thioether group, a halogen atom, a cyano group, an aldehyde group, a carbonyl group, a carboxy group, an oxycarbonyl group, an ester group, a carbamoyl group, an amide group, a sulfonyl group, a sulfonate ester group, a sulfonamide group, an imino group, an amino group, a nitro group, a silyl group, a siloxanyl group, a boryl group, or a phosphine oxide group. These substituents may be further substituted with the above-mentioned substituents.
[0044] The alkyl group refers to a saturated aliphatic hydrocarbon group such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, or a tert-butyl group, which may or may not have a substituent. When the alkyl group is substituted, the additional substituent is not particularly limited, and examples thereof include an alkyl group, a halogen atom, an aryl group, and a heteroaryl group, and this point is also applicable to the following description. The number of carbon atoms in the alkyl group is not particularly limited, but is preferably in the range of 1 to 20, more preferably 1 to 8, from the viewpoints of availability and cost.
[0045] The cycloalkyl group refers to a saturated alicyclic hydrocarbon group, such as a cyclopropyl group, a cyclohexyl group, a norbornyl group, an adamantyl group, or the like, which may or may not have a substituent. The number of carbon atoms in the alkyl group is not particularly limited, but is preferably in the range of 3 to 20.
[0046] The heterocyclic group refers to an aliphatic ring having atoms other than carbon atoms in the ring, such as a pyran ring, a piperidine ring, or a cyclic amide, which may or may not have a substituent. The number of carbon atoms in the heterocyclic group is not particularly limited, but is preferably in the range of 2 to 20.
[0047] The alkenyl group refers to an unsaturated aliphatic hydrocarbon group containing a double bond, such as a vinyl group, an allyl group, or a butadienyl group, which may or may not have a substituent. The number of carbon atoms in the alkenyl group is not particularly limited, but is preferably in the range of 2 to 20.
[0048] The cycloalkenyl group refers to an unsaturated alicyclic hydrocarbon group containing a double bond, such as a cyclopentenyl group, a cyclopentadienyl group, or a cyclohexenyl group, which may or may not have a substituent. The number of carbon atoms in the cycloalkenyl group is not particularly limited, but is preferably in the range of 3 to 20.
[0049] The alkynyl group refers to an unsaturated aliphatic hydrocarbon group containing a triple bond, such as an ethynyl group, which may or may not have a substituent. The number of carbon atoms in the alkynyl group is not particularly limited, but is preferably in the range of 2 to 20.
[0050] The alkoxy group refers to a functional group in which an aliphatic hydrocarbon group is bonded via an ether bond, such as a methoxy group, an ethoxy group, or a propoxy group, and this aliphatic hydrocarbon group may or may not have a substituent. The number of carbon atoms in the alkoxy group is not particularly limited, but is preferably in the range of 1 to 20.
[0051] An alkylthio group is an alkoxy group in which the oxygen atom of the ether bond is replaced with a sulfur atom. The hydrocarbon group of the alkylthio group may or may not have a substituent. The number of carbon atoms in the alkylthio group is not particularly limited, but is preferably in the range of 1 to 20.
[0052] The aryl ether group refers to a functional group in which an aromatic hydrocarbon group is bonded via an ether bond, such as a phenoxy group, and the aromatic hydrocarbon group may or may not have a substituent. The number of carbon atoms in the aryl ether group is not particularly limited, but is preferably in the range of 6 to 40.
[0053] An aryl thioether group is an aryl ether group in which the oxygen atom of the ether bond is substituted with a sulfur atom. The aromatic hydrocarbon group in the aryl thioether group may or may not have a substituent. The number of carbon atoms in the aryl thioether group is not particularly limited, but is preferably in the range of 6 to 40.
[0054] The aryl group refers to an aromatic hydrocarbon group such as a phenyl group, a biphenyl group, a terphenyl group, a naphthyl group, a fluorenyl group, a benzofluorenyl group, a dibenzofluorenyl group, a phenanthryl group, an anthracenyl group, a benzophenanthryl group, a benzanthracenyl group, a chrysenyl group, a pyrenyl group, a fluoranthenyl group, a triphenylenyl group, a benzofluoranthenyl group, a dibenzoanthracenyl group, a perylenyl group, or a helicenyl group. Among these, a phenyl group, a biphenyl group, a terphenyl group, a naphthyl group, a fluorenyl group, a phenanthryl group, an anthracenyl group, a pyrenyl group, a fluoranthenyl group, or a triphenylenyl group is preferred. The aryl group may or may not have a substituent. The number of carbon atoms in the aryl group is not particularly limited, but is preferably in the range of 6 to 40, more preferably 6 to 30.
[0055] The aryl group is preferably a phenyl group, a biphenyl group, a terphenyl group, a naphthyl group, a fluorenyl group, a phenanthryl group, or an anthracenyl group, more preferably a phenyl group, a biphenyl group, a terphenyl group, or a naphthyl group, even more preferably a phenyl group, a biphenyl group, or a terphenyl group, and particularly preferably a phenyl group.
[0056] When each of the substituents is further substituted with an aryl group, the aryl group is preferably a phenyl group, a biphenyl group, a terphenyl group, a naphthyl group, a fluorenyl group, a phenanthryl group, or an anthracenyl group, more preferably a phenyl group, a biphenyl group, a terphenyl group, or a naphthyl group, and particularly preferably a phenyl group.
[0057] Examples of heteroaryl groups include pyridyl, furanyl, thienyl, quinolinyl, isoquinolinyl, pyrazinyl, pyrimidyl, pyridazinyl, triazinyl, naphthyridinyl, cinnolinyl, phthalazinyl, quinoxalinyl, quinazolinyl, benzofuranyl, benzothienyl, indolyl, dibenzofuranyl, dibenzothienyl, carbazolyl, and benzocarbazolyl. It refers to a cyclic aromatic group having one or more atoms other than carbon in the ring, such as a benzoyl group, a carbolinyl group, an indolocarbazolyl group, a benzofurocarbazolyl group, a benzothienocarbazolyl group, a dihydroindenocarbazolyl group, a benzoquinolinyl group, an acridinyl group, a dibenzoacridinyl group, a benzimidazolyl group, an imidazopyridyl group, a benzoxazolyl group, a benzothiazolyl group, or a phenanthrolinyl group. However, a naphthyridinyl group refers to a 1,5-naphthyridinyl group, a 1,6-naphthyridinyl group, a 1,7-naphthyridinyl group, a 1,8-naphthyridinyl group, a 2,6-naphthyridinyl group, or a 2,7-naphthyridinyl group. The heteroaryl group may or may not have a substituent. The number of carbon atoms in the heteroaryl group is not particularly limited, but is preferably in the range of 2 or more and 40 or less, and more preferably 2 or more and 30 or less.
[0058] As the heteroaryl group, a pyridyl group, a furanyl group, a thienyl group, a quinolinyl group, a pyrimidyl group, a triazinyl group, a benzofuranyl group, a benzothienyl group, an indolyl group, a dibenzofuranyl group, a dibenzothienyl group, a carbazolyl group, a benzimidazolyl group, an imidazopyridyl group, a benzoxazolyl group, a benzothiazolyl group, or a phenanthrolinyl group is preferred, and a pyridyl group, a furanyl group, a thienyl group, or a quinolinyl group is more preferred, and a pyridyl group is particularly preferred.
[0059] When each substituent is further substituted with a heteroaryl group, the heteroaryl group is preferably a pyridyl group, a furanyl group, a thienyl group, a quinolinyl group, a pyrimidyl group, a triazinyl group, a benzofuranyl group, a benzothienyl group, an indolyl group, a dibenzofuranyl group, a dibenzothienyl group, a carbazolyl group, a benzimidazolyl group, an imidazopyridyl group, a benzoxazolyl group, a benzothiazolyl group, or a phenanthrolinyl group, more preferably a pyridyl group, a furanyl group, a thienyl group, or a quinolinyl group, and particularly preferably a pyridyl group.
[0060] The term "halogen" refers to an atom selected from fluorine, chlorine, bromine, and iodine. The carbonyl group, carboxy group, oxycarbonyl group, ester group, carbamoyl group, amide group, and imino group may or may not have a substituent. Examples of the substituent include an alkyl group, a cycloalkyl group, an aryl group, and a heteroaryl group, and these substituents may be further substituted.
[0061] The sulfonyl group, sulfonate group, and sulfonamide group are each represented by —S(═O)R 10 , -S(=O)2OR 10 , -S(=O)NR 10 R 11 R is a group represented by the formula: 10 , R 11 is a hydrogen atom or is selected from the same group as the substituents when substituted as described above.
[0062] The amino group is a substituted or unsubstituted amino group. In the case of substitution, examples of the substituent include an aryl group, a heteroaryl group, a linear alkyl group, and a branched alkyl group. As the aryl group and the heteroaryl group, a phenyl group, a naphthyl group, a pyridyl group, and a quinolinyl group are preferred. These substituents may be further substituted. The number of carbon atoms is not particularly limited, but is preferably in the range of 2 to 50, more preferably 6 to 40, and particularly preferably 6 to 30.
[0063] The silyl group refers to, for example, alkylsilyl groups such as trimethylsilyl group, triethylsilyl group, tert-butyldimethylsilyl group, propyldimethylsilyl group, and vinyldimethylsilyl group, and arylsilyl groups such as phenyldimethylsilyl group, tert-butyldiphenylsilyl group, triphenylsilyl group, and trinaphthylsilyl group. The substituent on silicon may be further substituted. The number of carbon atoms in the silyl group is not particularly limited, but is preferably in the range of 1 to 30.
[0064] The siloxanyl group refers to a silicon compound group via an ether bond, such as a trimethylsiloxanyl group. The substituent on the silicon may be further substituted. The boryl group refers to a substituted or unsubstituted boryl group. In the case of substitution, examples of the substituent include an aryl group, a heteroaryl group, a linear alkyl group, a branched alkyl group, an aryl ether group, an alkoxy group, and a hydroxyl group. Among these, an aryl group and an aryl ether group are preferred.
[0065] The phosphine oxide group is —P(═O)R 10 R 11 The R of the phosphine oxide group is a group represented by the formula: 10 and R 11 is a hydrogen atom or is selected from the same group as the substituents when substituted as described above.
[0066] (Polymer microparticles) The polymer microparticles according to an embodiment of the present invention (hereinafter sometimes abbreviated as polymer microparticles of the present invention) are polymer microparticles containing a resin as a main component and containing a light-emitting material or a coloring material. Specifically, the sphericity, which indicates the sphericity of the polymer microparticles of the present invention, is 80 or more and 100 or less. High sphericity can reduce optical loss due to unwanted light scattering on the surface of the polymer microparticles and multiple reflections inside the particles. Furthermore, it can suppress the promotion of deterioration of the light-emitting material or coloring material due to multiple excitation. The sphericity of the polymer microparticles of the present invention is preferably 85 or more and 100 or less, more preferably 90 or more and 100 or less, even more preferably 93 or more and 100 or less, and particularly preferably 95 or more and 100 or less.
[0067] The sphericity of the polymer microparticles of the present invention is determined by observing 30 particles randomly selected from a scanning electron microscope photograph and determining the minor axis and major axis of each of these particles according to the following formula.
[0068]
[0069] In this formula, S is sphericity, a is major axis, b is minor axis, and n is the number of measurements (n=30 in this embodiment).
[0070] In the polymer microparticles of the present invention, the D50 particle size is preferably in the range of 0.1 μm to 100 μm. If the D50 particle size exceeds 100 μm, the particle size of the polymer microparticles will be greater than the layer thickness of a film or the like used in optical materials, causing roughness and poor appearance. If the D50 particle size is less than 0.1 μm, the surface area of the polymer microparticles will be excessively large, which will cause an increase in viscosity when used in a slurry or ink, and is therefore undesirable.
[0071] The upper limit of the D50 particle size of the polymer microparticles of the present invention is preferably 70 μm or less, more preferably 50 μm or less, even more preferably 30 μm or less, particularly preferably 20 μm or less, significantly preferably 10 μm or less, and most preferably 5.0 μm or less. The lower limit of the D50 particle size is preferably 0.2 μm or more, more preferably 0.5 μm or more, and even more preferably 1.0 μm or more.
[0072] In the present invention, the D50 particle size of the polymer microparticles is the particle size (D50 particle size) at which the cumulative frequency from the small particle size side in the particle size distribution (particle size distribution) of the polymer microparticles measured by a laser diffraction particle size distribution meter is 50%.
[0073] The particle size distribution of the polymer microparticles of the present invention is expressed as the ratio of the D90 particle size to the D10 particle size in the particle size distribution, i.e., D90 particle size / D10 particle size (hereinafter referred to as D90 / D10). In the polymer microparticles of the present invention, D90 / D10 is preferably 1.0 or more and 5.0 or less. A narrow particle size distribution of the polymer microparticles is preferable because it eliminates the difference in light scattering properties due to the difference in particle size and provides better optical uniformity. Therefore, the upper limit of D90 / D10 is more preferably 4.0 or less, and even more preferably 3.0 or less. In addition, from the viewpoint of excellent packing ability in a powder state, the lower limit of D90 / D10 is more preferably 1.5 or more, and even more preferably 2.0 or more.
[0074] In the present invention, D90 / D10 of polymer microparticles is a value obtained by dividing the particle diameter (D90 particle diameter) at which the cumulative frequency from the small particle diameter side in the particle size distribution of the polymer microparticles measured by the above-mentioned laser diffraction particle size distribution meter is 90% by the particle diameter (D10 particle diameter) at which the cumulative frequency from the small particle diameter side in the particle size distribution is 10%.
[0075] The smoothness of the surface of the polymer microparticles of the present invention can be expressed by the amount of linseed oil that the polymer microparticles absorb (hereinafter referred to as linseed oil absorption). That is, the smoother the surface of the polymer microparticles, the fewer or no pores there are on the surface, and the lower the linseed oil absorption.
[0076] The polymer microparticles of the present invention preferably have a linseed oil absorption of 1 mL / 100 g or more and 200 mL / 100 g or less. A lower linseed oil absorption of the polymer microparticles is preferable because it results in a smooth surface and a solid interior, thereby reducing undesired light scattering at the particle surface and optical loss due to multiple reflections inside the particles. Furthermore, the lower the linseed oil absorption of the polymer microparticles, the more effectively they can suppress the accelerated deterioration of luminescent materials and coloring materials due to multiple excitation. Furthermore, thickening can be reduced when the polymer microparticles are used in slurries or inks. Therefore, the linseed oil absorption of the polymer microparticles is more preferably 1 mL / 100 g or more and 150 mL / 100 g or less, even more preferably 1 mL / 100 g or more and 120 mL / 100 g or less, even more preferably 1 mL / 100 g or more and 100 mL / 100 g or less, and particularly preferably 1 mL / 100 g or more and 70 mL / 100 g or less. The lower limit of the linseed oil absorption is preferably as low as possible.
[0077] The linseed oil absorption of the polymer microparticles is measured in accordance with Japanese Industrial Standards (JIS) JIS K 5101 (2004) "Pigment Test Method: Refined Linseed Oil Method."
[0078] Furthermore, in the polymer microparticles of the present invention, the surface smoothness and internal solidity can be expressed by the BET specific surface area determined by gas adsorption. Specifically, the smoother the surface of the polymer microparticles, the smaller the BET specific surface area of the polymer microparticles, and the more solid the interior of the polymer microparticles, the smaller the BET specific surface area of the polymer microparticles. If the surface of the polymer microparticles is smooth and the interior of the polymer microparticles is solid, it is possible to reduce optical loss due to undesired light scattering on the particle surface and multiple reflections inside the particles, and it is also possible to suppress the promotion of deterioration of luminescent materials and coloring materials due to multiple excitation. Furthermore, since the surface area of the polymer microparticles is reduced and their fluidity is improved, the polymer microparticles are easy to handle. Therefore, it is preferable that the BET specific surface area of the polymer microparticles is as small as possible. Specifically, the BET specific surface area of the polymer microparticles is 10 m 2 / g or less, and 2 / g or less is more preferable, and 2 / g or less is more preferable, 2 The lower limit of the BET specific surface area is theoretically 0.05 m / g when the particle diameter of the polymer fine particles is 100 μm. 2 / g.
[0079] The BET specific surface area of the polymer fine particles is measured in accordance with Japanese Industrial Standards (JIS) JIS R 1626 (1996) "Method for measuring specific surface area by gas adsorption BET method."
[0080] The solidity of the polymer microparticles of the present invention can also be evaluated by the following formula, which shows the ratio of the theoretical surface area calculated from the BET specific surface area and the D50 particle size. The closer the R value in the formula below is to 1, the more gas adsorption occurs only on the outermost surface of the particle, indicating that the polymer microparticles are solid particles with a smooth surface. In the polymer microparticles of the present invention, the R value in the formula below is preferably 5 or less, more preferably 4 or less, even more preferably 3 or less, and most preferably 2 or less. Theoretically, the lower limit of the R value is 1.
[0081]
[0082] In this formula, R is the surface area ratio, D is the D50 particle diameter, α is the density of the polymer particles, and A is the BET specific surface area.
[0083] (Resin in Polymer Microparticles) As described above, the polymer microparticles of the present invention are polymer microparticles containing a resin as a main component and containing a light-emitting material or a coloring material. In such polymer microparticles, materials with excellent transparency and heat resistance are preferably used as the resin constituting the particles. Examples of the resin include photocurable resist materials having reactive vinyl groups, such as acrylic acid-based, methacrylic acid-based, polyvinyl cinnamate-based, and cyclic rubber-based materials, epoxy resins, silicone resins (including organopolysiloxane cured products (crosslinked products) such as silicone rubber and silicone gel), urea resins, fluororesins, polycarbonate resins, acrylic resins, urethane resins, melamine resins, polyvinyl resins, polyamide resins, phenolic resins, polyvinyl alcohol resins, cellulose resins, aliphatic ester resins, aromatic ester resins, aliphatic polyolefin resins, and aromatic polyolefin resins. Furthermore, the resin contained as the main component in the polymer microparticles of the present invention may be a mixture or copolymer of these resins. By appropriately designing these resins, resins useful for the polymer microparticles of the present invention can be obtained.
[0084] Among these resins, from the viewpoint of transparency and dispersibility of light-emitting materials or coloring materials, any of acrylic resins, copolymer resins containing acrylic ester or methacrylic ester moieties, polyester resins, cycloolefin resins, epoxy resins, and silicone resins is preferred. More preferred are acrylic resins, copolymer resins containing acrylic ester or methacrylic ester moieties, and polyester resins, and particularly preferred are acrylic resins, copolymer resins containing acrylic ester or methacrylic ester moieties. Furthermore, from the viewpoint of heat resistance, thermosetting resins and photocurable resins can be suitably used.
[0085] Furthermore, the polymer microparticles of the present invention are primarily comprised of a resin having at least one ring structure selected from the group consisting of an aliphatic hydrocarbon ring, an aliphatic heterocycle, and a ring containing SP3 carbon. When the resin serving as the primary component has at least one ring structure in its molecular structure, the molecular motion of the resin is suppressed, thereby suppressing changes in the dispersion state of the luminescent material or coloring material in the polymer microparticles, thereby preventing the proximity of these materials. Furthermore, when the ring structure in the molecular structure of the resin is at least one ring structure selected from the group consisting of an aliphatic hydrocarbon ring, an aliphatic heterocycle, and a ring containing SP3 carbon, the π-conjugated structure in the resin is reduced, thereby reducing the generation of active species due to light absorption. This suppresses deterioration of the luminescent material or coloring material in the polymer microparticles, thereby preventing a deterioration in the durability of the polymer microparticles. Here, SP3 carbon refers to a carbon atom bonded to four atoms via an SP3 hybrid orbital.
[0086] The number of atoms constituting the above-mentioned aliphatic hydrocarbon ring, aliphatic heterocycle, and ring containing SP3 carbon is not particularly limited, but is usually in the range of 3 to 30, preferably 4 to 20, and more preferably 5 to 15.
[0087] Specific examples of the ring structure containing aliphatic hydrocarbon ring, aliphatic heterocycle and SP3 carbon include cyclobutane, cyclopentane, cyclohexane, norbornene, adamantane, pyrrolidine, piperidine, ethylene oxide, oxetane, furan, tetrahydropyran, morpholine, dioxane, indane, fluorene, cyclic ester, cyclic amide and derivatives thereof.Among these, cyclohexane, norbornene, adamantane, ethylene oxide, oxetane, fluorene, cyclic ester, cyclic amide and derivatives thereof are preferred, cyclohexane, norbornene, adamantane, fluorene, cyclic ester and derivatives thereof are more preferred, cyclohexane, norbornene, fluorene, cyclic ester and derivatives thereof are even more preferred, and cyclohexane, norbornene and derivatives thereof are particularly preferred.
[0088] In the polymer microparticles of the present invention, the resin that is the main component is preferably at least one of the first and second resins shown below. The first resin is a resin having at least one ring structure selected from the group consisting of an aliphatic hydrocarbon ring, an aliphatic heterocycle, and a ring containing an SP3 carbon in the polymer main chain. The second resin is a resin in which at least one ring structure selected from the group consisting of an aliphatic hydrocarbon ring, an aliphatic heterocycle, and a ring containing an SP3 carbon is directly linked to the polymer main chain. When the at least one ring structure is contained in the polymer main chain or is directly linked to the polymer main chain, molecular motion of the resin can be suppressed more efficiently than when the ring structure is introduced into a polymer side chain. This makes it possible to suppress changes in the dispersion state of the light-emitting material or coloring material in the polymer microparticles.
[0089] In the polymer microparticles of the present invention, in order to disperse the light-emitting material or coloring material well in the resin, it is preferable that the resin (the main component resin) has both a partial structure that is highly compatible with the light-emitting material or coloring material and a partial structure that is less compatible with the light-emitting material or coloring material. A more preferable form of the resin is, for example, a copolymer that randomly contains a partial structure that is highly compatible with the light-emitting material or coloring material and a partial structure that is less compatible with the light-emitting material or coloring material.
[0090] Examples of partial structures that are highly compatible with light-emitting materials or coloring materials include, but are not limited to, moieties derived from acrylic acid, methacrylic acid, acrylic acid esters, and methacrylic acid esters, as well as moieties linked by ester bonds or amide bonds. On the other hand, examples of partial structures that are poorly compatible with light-emitting materials or coloring materials include, but are not limited to, moieties derived from vinyl compounds consisting only of carbon atoms and vinyl compounds having aliphatic hydrocarbon rings. Therefore, it is preferable that the resin that is the main component has at least one of a moiety derived from acrylic acid, methacrylic acid, acrylic acid esters, or methacrylic acid esters, and a moiety linked by ester bonds or amide bonds, and at least one of a moiety derived from a vinyl compound consisting only of carbon atoms and a moiety derived from a vinyl compound having aliphatic hydrocarbon rings.
[0091] From the viewpoint of ensuring compatibility between the resin as the main component and the light-emitting material or coloring material and dispersing these materials well in the resin, the content of the partial structure having high compatibility with the light-emitting material or coloring material in the copolymer as the resin is preferably 30 wt % or more, more preferably 50 wt % or more, and even more preferably 70 wt % or more of the total amount of the resin. On the other hand, the content of the partial structure having low compatibility with the light-emitting material or coloring material in the copolymer as the resin is preferably 70 wt % or less, more preferably 50 wt % or less, and even more preferably 30 wt % or less of the total amount of the resin.
[0092] Suitable examples of the resin that is the main component include, but are not limited to, a resin having a partial structure represented by general formula (1) and a partial structure represented by general formula (2) in its molecular structure.
[0093]
[0094] In general formula (1), Y 1 and Y 2 may be the same or different and are a hydrogen atom or an organic group having 1 to 20 carbon atoms. 3 ~Y 6 may be the same or different and each represents a hydrogen atom or an organic group having 1 to 20 carbon atoms, and Y 3 ~Y 6 At least one of the groups is a group containing an aliphatic cyclic hydrocarbon structure.
[0095] Y in general formula (1) 1 is preferably a hydrogen atom or a methyl group from the viewpoint of good copolymerization reactivity, and more preferably a methyl group from the viewpoint of reducing radical generation.
[0096] Y in general formula (1) 2From the viewpoint of improving the heat resistance of the resin, Y is preferably a hydrogen atom, an alkyl group, a cycloalkyl group, a heterocyclic group, an alkenyl group, a cycloalkenyl group, an alkynyl group, a hydroxyl group, a thiol group, an alkoxy group, an alkylthio group, an aryl ether group, an aryl thioether group, an aryl group, or a heteroaryl group. These groups may be further substituted with the above-mentioned substituents. Among these, Y 2 is more preferably a methyl group or a cycloalkyl group. From the viewpoint of compatibility with the light-emitting material or the coloring material, Y 2 is more preferably a methyl group.
[0097] Y in general formula (2) 3 ~Y 6 From the viewpoint of improving the heat resistance of the resin, is preferably a hydrogen atom, an alkyl group, a cycloalkyl group, a heterocyclic group, an alkenyl group, a cycloalkenyl group, an alkynyl group, a hydroxyl group, a thiol group, an alkoxy group, an alkylthio group, an aryl ether group, an aryl thioether group, an aryl group, or a heteroaryl group. These groups may be further substituted with the above-mentioned substituents.
[0098] As described above, Y in general formula (2) 3 ~Y 6 At least one of the Y is a group containing an aliphatic cyclic hydrocarbon structure. 3 ~Y 6 At least one of these Y is preferably a substituted or unsubstituted cyclohexyl group. 3 ~Y 6 It is more preferable that one of the groups is a substituted or unsubstituted cyclohexyl group, and the other three are hydrogen atoms.
[0099] The content of the repeating unit of the partial structure represented by general formula (1) is not particularly limited, but is preferably 30 wt % or more, more preferably 50 wt % or more, even more preferably 60 wt % or more, and particularly preferably 70 wt % or more of the total amount of the resin that is the main component. By having the proportion of the repeating unit of the partial structure represented by general formula (1) in the above range, compatibility between the resin and the light-emitting material or coloring material can be ensured, and these materials can be well dispersed in the resin.
[0100] The content of the repeating unit of the partial structure represented by general formula (1) is preferably 95 wt % or less, more preferably 90 wt % or less, and even more preferably 85 wt % or less, of the total amount of the resin that is the main component. By having the proportion of the repeating unit of the partial structure represented by general formula (1) in the above range, compatibility between the resin and the light-emitting material or coloring material can be ensured, and these materials can be well dispersed in the resin.
[0101] The content of the repeating unit of the partial structure represented by general formula (2) is preferably 5 wt % or more, more preferably 10 wt % or more, and particularly preferably 15 wt % or more, of the total amount of the resin that is the main component. By having the content of the repeating unit of the partial structure represented by general formula (2) in the above range, compatibility between the resin and the light-emitting material or coloring material can be ensured, and these materials can be well dispersed in the resin.
[0102] The content of the repeating unit of the partial structure represented by general formula (2) is preferably 70 wt % or less, more preferably 50 wt % or less, and even more preferably 30 wt % or less, of the total amount of the resin that is the main component. By having the proportion of the repeating unit of the partial structure represented by general formula (2) in the above range, compatibility between the resin and the light-emitting material or coloring material can be ensured, and these materials can be well dispersed in the resin.
[0103] Furthermore, in the polymer microparticles of the present invention, the lower limit of the glass transition temperature (Tg) of the resin that is the main component thereof is not particularly limited, but is preferably 80°C or higher, and more preferably 100°C or higher. When the Tg of the resin is 100°C or higher, molecular motion of the resin due to heat from incident light from a light source or heat from operating the device is further suppressed, and changes in the dispersion state of the luminescent material or coloring material in the resin are suppressed even under high temperature conditions. The lower limit of the Tg of the resin is more preferably 110°C or higher, and even more preferably 120°C or higher. The upper limit of the Tg of the resin is not particularly limited. However, if the crystallinity of the resin is excessively high, the dispersibility of the luminescent material or coloring material in the resin will deteriorate, so the upper limit of the Tg of the resin is preferably 180°C or lower.
[0104] The glass transition temperature of the thermoplastic resin can be measured using a commercially available measuring device (for example, a differential scanning calorimeter (trade name: DSCQ20) manufactured by TA Instruments) at a temperature rise rate of 20°C / min. The measurement sample is not particularly limited as long as it is placed in a measurement container, but it is preferable to measure the sample in the form of powder or fine particles, or in a state in which the resin solution has been cast and then thoroughly dried to remove the solvent.
[0105] In the polymer microparticles of the present invention, the lower limit of the weight-average molecular weight (Mw) of the resin that is the main component thereof is preferably 5,000 or more, more preferably 15,000 or more, and even more preferably 20,000 or more. The upper limit of the weight-average molecular weight is preferably 500,000 or less, more preferably 100,000 or less, and even more preferably 50,000 or less. If the weight-average molecular weight is within the above range, the uniformity of the shape and particle size will be high when the particles are molded into particles.
[0106] Here, the weight average molecular weight can be measured in terms of polystyrene by performing GPC analysis using a commercially available measuring device (for example, a GPC analyzer manufactured by Tosoh Corporation (trade name: HLC-8220)) based on Japanese Industrial Standards (JIS) K7252-3 (2008).
[0107] Furthermore, in the polymer microparticles of the present invention, the resin that is the main component thereof preferably has a light transmittance of 85% or more in the wavelength range of 400 nm to 800 nm. The higher the light transmittance, the more transparent the resin becomes, and the smaller the optical loss can be when polymer microparticles containing the resin are used as a constituent material for a light source unit, etc. The light transmittance is preferably 87% or more, more preferably 90% or more, even more preferably 91% or more, and particularly preferably 92% or more.
[0108] The light transmittance of the resin in the wavelength range of 400 nm to 800 nm can be measured by preparing a resin sample piece having a film thickness of 1 μm to 100 μm and using a commercially available measuring instrument (for example, a violet-visible spectrophotometer (trade name U-3010) manufactured by Hitachi, Ltd.).
[0109] The resin, which is the main component, has an intrinsic birefringence of −30×10 -4 Above + 30 x 10 -4 The smaller the absolute value of the intrinsic birefringence of the resin, the more the diffusion of light in the resin can be prevented. The intrinsic birefringence of the resin is preferably −25×10 -4 Above + 25 x 10 -4 It is preferable that the value is less than or equal to -20×10 -4 Above + 20 x 10 -4 More preferably, it is less than or equal to -15 x 10 -4 Above + 15 x 10 -4 More preferably, it is less than or equal to -10 x 10 -4 Above + 10 x 10 -4 It is even more preferred that:
[0110] The intrinsic birefringence of the resin described above can be calculated by calculating the dielectric polarization difference in each bonding unit of the structural units using a molecular orbital method such as the AM1 method or PM3 method, and then calculating the volume average value (intrinsic birefringence value) using the following Lorentz-Lorentz equation.
[0111]
[0112] In this formula, Δn0 is the intrinsic birefringence value, ΔP is the difference between the dielectric polarizability in the direction of the molecular chain axis and the dielectric polarizability in the direction perpendicular to the molecular chain axis, n is the refractive index, d is the density, N is Avogadro's number, and M is the molecular weight.
[0113] Resins useful for the polymer microparticles of the present invention can be obtained, for example, by copolymerizing the raw material monomers in the presence of a polymerization initiator and a catalyst. Alternatively, commercially available resins can be used. Examples of commercially available resins include, but are not limited to, Optimas (registered trademark) 6500, Optimas (registered trademark) 7500, and Iupizeta (registered trademark) EP-5000 manufactured by Mitsubishi Gas Chemical Company, Inc., and OKP (registered trademark) 4 and OKP (registered trademark)-A1 manufactured by Osaka Gas Chemicals Co., Ltd. In addition, resins disclosed in JP-A-2021-162621, JP-A-2022-116643, JP-A-2022-179996, JP-A-2022-72382, JP-A-2020-180184, JP-A-2018-53044, etc. can also be suitably used.
[0114] (Light-emitting material or coloring material) As described above, the polymer microparticles of the present invention are microparticles containing a resin as a main component and a light-emitting material or a coloring material. Specific examples of light-emitting materials or coloring materials that are suitable for use in the polymer microparticles of the present invention include, for example, inorganic fluorescent materials, organic pigments, organic dyes, and quantum dots. The polymer microparticles of the present invention may contain two or more of these as the light-emitting material or coloring material. Among these, it is more preferable to use an organic pigment or an organic dye from the viewpoints of high dispersibility in the resin, reduced usage amount, and reduced environmental impact. Organic dyes are even more preferable.
[0115] Suitable examples of the organic pigment or organic dye include compounds having a fused aryl ring or derivatives thereof, compounds having a heteroaryl ring or derivatives thereof, borane derivatives, stilbene derivatives, aromatic acetylene derivatives, tetraphenylbutadiene derivatives, aldazine derivatives, pyrromethene derivatives, diketopyrrolo[3,4-c]pyrrole derivatives, coumarin derivatives, azole derivatives and metal complexes thereof, cyanine compounds, xanthene compounds, thioxanthene compounds, polyphenylene compounds, naphthalimide derivatives, phthalocyanine derivatives and metal complexes thereof, porphyrin derivatives and metal complexes thereof, oxazine compounds, helicene compounds, aromatic amine derivatives, and organometallic complex compounds.
[0116] Examples of compounds having a fused aryl ring and derivatives thereof include naphthalene, anthracene, phenanthrene, pyrene, chrysene, naphthacene, triphenylene, perylene, fluoranthene, fluorene, indene, etc. Examples of compounds having a heteroaryl ring and derivatives thereof include furan, pyrrole, thiophene, silole, 9-silafluorene, 9,9'-spirobisilafluorene, benzothiophene, benzofuran, indole, dibenzothiophene, dibenzofuran, imidazopyridine, phenanthroline, pyridine, pyrazine, naphthyridine, quinoxaline, pyrrolopyridine, etc.
[0117] Examples of stilbene derivatives include 1,4-distyrylbenzene, 4,4'-bis(2-(4-diphenylaminophenyl)ethenyl)biphenyl, and 4,4'-bis(N-(stilben-4-yl)-N-phenylamino)stilbene. Examples of coumarin derivatives include coumarin 6, coumarin 7, and coumarin 153. Examples of azole derivatives and metal complexes thereof include imidazole, thiazole, thiadiazole, carbazole, oxazole, oxadiazole, and triazole.
[0118] Examples of cyanine compounds include indocyanine green. Examples of xanthene compounds and thioxanthene compounds include fluorescein, eosin, and rhodamine. Examples of oxazine compounds include Nile red and Nile blue. Examples of aromatic amine derivatives include N,N'-diphenyl-N,N'-di(3-methylphenyl)-4,4'-diphenyl-1,1'-diamine. Examples of organometallic complex compounds include iridium (Ir), ruthenium (Ru), rhodium (Rh), palladium (Pd), platinum (Pt), osmium (Os), and rhenium (Re).
[0119] Among the above-mentioned organic pigments or organic dyes, perylene derivatives, xanthene compounds, pyrromethene derivatives, diketopyrrolo[3,4-c]pyrrole derivatives, coumarin derivatives, phthalocyanine derivatives and metal complexes thereof, and porphyrin derivatives and metal complexes thereof are more preferred because they have a large absorption coefficient and relatively high heat resistance.
[0120] In the polymer fine particles of the present invention, the light-emitting material or the coloring material has a molar absorption coefficient of 10,000 M at the maximum absorption wavelength in the wavelength range of 300 nm or more. -1 ・cm -1 It is preferable that the organic material contains at least one organic material having a molar absorption coefficient of 20,000 M or more. These materials have a large molar absorption coefficient, so that light can be efficiently absorbed. The molar absorption coefficient is more preferably 20,000 M or more. -1 ・cm -1 More preferably, 30,000M -1 ・cm -1 More preferably, 50,000M -1 ・cm -1 That's all. Suitable organic materials with a large molar absorption coefficient include perylene derivatives, xanthene compounds, pyrromethene derivatives, diketopyrrolo[3,4-c]pyrrole derivatives, coumarin derivatives, phthalocyanine derivatives and metal complexes thereof, and porphyrin derivatives and metal complexes thereof. However, the organic materials are not particularly limited to these.
[0121] In one embodiment of the polymer microparticles of the present invention, the polymer microparticles contain at least one luminescent material, and the luminescent material preferably has an emission spectrum with a half-width of 60 nm or less. In this case, the polymer microparticles of the present invention can absorb incident light and convert the absorbed incident light into light with high color purity and a wavelength different from that of the incident light. The luminescent material more preferably has an emission spectrum with a half-width of 50 nm or less, even more preferably has an emission spectrum with a half-width of 40 nm or less, and particularly preferably has an emission spectrum with a half-width of 30 nm or less.
[0122] The luminescent material contained in the polymer microparticles of the present invention is preferably at least one of the compounds represented by general formula (3), the compounds represented by general formula (4), and the compounds represented by general formula (5), since these materials exhibit luminescence with high color purity.
[0123]
[0124] In the general formula (3), X is C—R 7 Or N. 1 ~R 9 may be the same or different and are selected from a hydrogen atom, an alkyl group, a cycloalkyl group, a heterocyclic group, an alkenyl group, a cycloalkenyl group, an alkynyl group, an aryl group, a heteroaryl group, a hydroxyl group, a thiol group, an alkoxy group, an alkylthio group, an aryl ether group, an aryl thioether group, a halogen atom, a cyano group, an aldehyde group, a carbonyl group, a carboxy group, an oxycarbonyl group, an ester group, a carbamoyl group, an amide group, a sulfonyl group, a sulfonate ester group, a sulfonamide group, an amino group, an imino group, a nitro group, a silyl group, a siloxanyl group, a boryl group, a phosphine oxide group, and a fused ring or an aliphatic ring formed between adjacent substituents.
[0125]
[0126] In general formula (4) and general formula (5), ring Za, ring Zb, and ring Zc are each independently a substituted or unsubstituted aryl ring having 6 to 30 ring carbon atoms, or a substituted or unsubstituted heteroaryl ring having 5 to 30 ring carbon atoms.
[0127] In general formula (4), Z 1 and Z 2 are each independently an oxygen atom, NRa (a nitrogen atom having a substituent Ra), or a sulfur atom. 1 When R is NRa, the substituent R may be bonded to the ring Za or the ring Zb to form a ring. 2 When R is NRa, the substituent R may be bonded to the ring Z or the ring Zc to form a ring. E is a boron atom, a phosphorus atom, SiRa (a silicon atom having a substituent R), or P=O.
[0128] In the general formula (5), E 1 and E 2 are each independently BRa (boron atom having a substituent Ra), PRa (phosphorus atom having a substituent Ra), SiRa2 (silicon atom having two substituents Ra), P(=O)Ra2 (phosphine oxide having two substituents Ra) or P(=S)Ra2 (phosphine sulfide having two substituents Ra), C=O (carbonyl group), S(=O) or S(=O)2. E 1 When is BRa, PRa, SiRa2, P(=O)Ra2 or P(=S)Ra2, the substituent Ra may be bonded to ring Za or ring Zb to form a ring. 2 When is BRa, PRa, SiRa2, P(=O)Ra2 or P(=S)Ra2, the substituent Ra may be bonded to ring Za or ring Zc to form a ring.
[0129] The above-mentioned substituents Ra are each independently selected from the group consisting of a hydrogen atom, an alkyl group, a cycloalkyl group, a heterocyclic group, an alkenyl group, a cycloalkenyl group, an alkynyl group, an aryl group, a heteroaryl group, a hydroxyl group, a thiol group, an alkoxy group, an alkylthio group, an aryl ether group, an aryl thioether group, a halogen atom, a cyano group, an aldehyde group, a carbonyl group, a carboxy group, an oxycarbonyl group, an ester group, a carbamoyl group, an amide group, a sulfonyl group, a sulfonate ester group, a sulfonamide group, an amino group, an imino group, a nitro group, a silyl group, a siloxanyl group, a boryl group, a phosphine oxide group, and a fused ring and an aliphatic ring formed between adjacent substituents. The substituents Ra may be further substituted with a substituent selected from these. The substituents substituting the substituents Ra may be further substituted with a substituent selected from these.
[0130] In addition, in the general formula (3), the fused ring and the aliphatic ring formed between adjacent substituents may be any two adjacent substituents (for example, R 2 and R 3 ) are bonded to each other to form a conjugated or non-conjugated cyclic skeleton. In the compound represented by general formula (3), such a fused ring or aliphatic ring may be formed. The constituent elements of such a fused ring or aliphatic ring may include, in addition to carbon, an element selected from nitrogen, oxygen, sulfur, phosphorus, and silicon. Furthermore, the above-mentioned fused ring or aliphatic ring may be further fused with another ring.
[0131] In general formula (3), R 8 and R 9 is preferably fluorine, a fluorine-containing alkyl group, a fluorine-containing heteroaryl group or a fluorine-containing aryl group, a fluorine-containing alkoxy group, a fluorine-containing aryloxy group, a fluorine-containing heteroaryloxy group, or a cyano group. In particular, R is preferred because it is stable to excitation light and can provide a higher fluorescence quantum yield. 8 and R 9 is more preferably a fluorine atom or a cyano group.
[0132] In addition, in the general formula (3), X is C—R7 In addition, from the viewpoint of providing a higher fluorescence quantum yield and being less susceptible to thermal decomposition, and from the viewpoint of photostability, it is preferable that X is C—R 7 and R 7 is preferably a substituted or unsubstituted aryl group or a substituted or unsubstituted heteroaryl group, and is preferably a substituted or unsubstituted phenyl group, since this can prevent a decrease in photostability due to an excessively large twist of the carbon-carbon bond.
[0133] In addition, as another embodiment of the compound represented by general formula (3), R 1 and R 2 , R 2 and R 3 , R 4 and R 5 , and R 5 and R 6 At least one of the four pairs is preferably a ring structure represented by any one of the following general formulas (6A) to (6D). Each ring structure represented by each of general formulas (6A) to (6D) has a double bond. Therefore, by introducing any one of these ring structures into the compound, conjugation can be extended and the emission wavelength can be made longer. Furthermore, the ring structure introduced into the compound can fix the double bond site to the central skeleton by a chemical bond, thereby suppressing excessive structural relaxation in the excited state and enabling emission of excellent color purity.
[0134]
[0135] In general formulas (6A) to (6D), R 101 , R 102 and R 201 ~R 204 is R in general formula (3). 1 ~R 7 In general formula (6D), Ar is a substituted or unsubstituted aromatic hydrocarbon ring, or a substituted or unsubstituted aromatic heterocycle. In each of the ring structures represented by general formulas (6A) to (6D), R 101 and R 102 and may form a ring. * in the general formulae (6A) to (6D) indicates a linking portion with the pyrromethene skeleton.
[0136] In the ring structure represented by general formula (6D), Ar is preferably a substituted or unsubstituted benzene ring, a substituted or unsubstituted naphthalene ring, a substituted or unsubstituted phenanthrene ring, a substituted or unsubstituted pyridine ring, a substituted or unsubstituted pyrimidine ring, or a substituted or unsubstituted pyrazine ring. Furthermore, when Ar is a substituted or unsubstituted benzene ring, it is preferable because thermal and photochemical stability is improved.
[0137] In addition, in each of the ring structures represented by the general formulae (6A) to (6D), R 101 and R 102 and may form a ring. 101 and R 102 By forming a ring, structural relaxation is suppressed, and sharp light emission can be obtained. In addition, thermal vibration of the entire molecule is suppressed, improving thermal stability. 101 and R 102 A preferred example of a ring formed by R is a spirofluorene ring. 101 and R 102 Both are benzene rings, and they form a ring structure.
[0138] A first preferred example of the compound represented by general formula (3) is R 1 , R 3 , R 4 and R 6 may be the same or different and are each a substituted or unsubstituted phenyl group, and X is C—R 7 and R 7 is a substituted or unsubstituted phenyl group. 1 , R 3 , R 4 , R 6 and R 7 More preferably, at least one of the groups is a phenyl group substituted with a methoxy group.
[0139] A second preferred example of the compound represented by general formula (3) is R 1 , R 3 , R 4and R 6 may be the same or different and are substituted or unsubstituted alkyl groups, and X is C—R 7 and R 7 is a substituted or unsubstituted phenyl group. 2 and R 5 may be the same or different, and are more preferably substituted or unsubstituted ester groups, and even more preferably substituted or unsubstituted aryl ester groups.
[0140] A third preferred example of the compound represented by general formula (3) is R 2 and R 3 is a ring structure represented by general formula (6D), Ar in general formula (6D) is a substituted or unsubstituted benzene ring, and R in general formula (6D) 101 and R 102 may be the same or different and are a substituted or unsubstituted alkyl group or a substituted or unsubstituted phenyl group, and X is C—R 7 and R 7 is a substituted or unsubstituted phenyl group. 4 and R 6 may be the same or different, and are more preferably substituted or unsubstituted phenyl groups. 101 and R 102 It is also preferred that these form a ring.
[0141] In general formulas (4) and (5), examples of the substituted or unsubstituted aryl ring having 6 to 30 ring carbon atoms in ring Za, ring Zb, and ring Zc include aromatic hydrocarbon rings such as a benzene ring, a naphthalene ring, a phenanthrene ring, a chrysene ring, an anthracene ring, and a pyrene ring. Of these, a benzene ring is preferred from the viewpoint of ensuring solubility. Furthermore, examples of heteroaryl rings having 5 to 30 ring carbon atoms include aromatic heteroaryl ring structures such as a pyridine ring, a quinoline ring, and a phenanthroline ring. Of these, a pyridine ring is preferred from the viewpoints of ease of raw material availability and difficulty of synthesis.
[0142] In general formula (4) and general formula (5), the substituent Ra is preferably a group having 6 to 40 carbon atoms, including the substituent. The substituent Ra is preferably a substituted or unsubstituted aryl group, a substituted or unsubstituted heteroaryl group, or a substituted or unsubstituted alkyl group, and more preferably a substituted or unsubstituted aryl group. Examples of the substituted or unsubstituted aryl group include a substituted or unsubstituted phenyl group, a substituted or unsubstituted biphenyl group, a substituted or unsubstituted fluorenyl group, a substituted or unsubstituted naphthyl group, and a substituted or unsubstituted phenanthrenyl group. Among these, a substituted or unsubstituted phenyl group is more preferred.
[0143] In general formula (4), Z 1 and Z 2 is preferably an oxygen atom or NRa. This is because the π-conjugated system of the compound represented by general formula (4) is efficiently expanded, and the photoexcitation efficiency is increased. Similarly, E in general formula (4) is preferably a boron atom, and E in general formula (5) is preferably a boron atom. 1 and E 2 is preferably BRa, since the π-conjugated system is efficiently expanded.
[0144] In addition, in general formula (4) and general formula (5), ring Za, ring Zb, and ring Zc are preferably benzene rings, because the π-conjugated system of the compound represented by general formula (4) or general formula (5) can be efficiently expanded.
[0145] In the compound represented by general formula (4) or general formula (5), as described in, for example, the literature Adv. Mater., 2016, 28, 2777-2781, by optimally arranging an electron-donating amine nitrogen atom and an electron-accepting boron atom, it is possible to separate the HOMO orbital and the LUMO orbital by the multiple resonance effect. From the viewpoint of clearly separating the HOMO orbital and bringing the singlet excited state and the triplet excited state closer to each other, thereby facilitating the emission of delayed fluorescence, in general formula (4), E is a boron atom with strong electron-accepting properties, and Z 1 and Z 2are preferably both NRa groups having strong electron donating properties.
[0146] Furthermore, it is more preferable that the substituent Ra in the general formula (4) and the general formula (5) forms a structure in which it is bonded to at least one of the rings Za, Zb, and Zc, because the substituent Ra is bonded to at least one of the rings Za, Zb, and Zc, and thus E in the general formula (4) or E in the general formula (5) can be bonded to at least one of the rings Za, Zb, and Zc. 1 and E 2 This is because it is expected that the steric protection effect of the compound will be further enhanced, and the effect of suppressing a decrease in the fluorescence quantum yield will be further improved.
[0147] Examples of compounds represented by general formula (3), compounds represented by general formula (4), and compounds represented by general formula (5) are shown below, but the compounds are not limited to these.
[0148]
[0149]
[0150]
[0151]
[0152]
[0153] In addition, examples of organic pigments or organic dyes other than the compounds represented by general formula (3), the compounds represented by general formula (4), and the compounds represented by general formula (5) are shown below. However, the organic pigments or organic dyes are not particularly limited to these. For example, compounds disclosed in JP-T-2014-519191, JP-T-2016-534100, JP-T-2017-523124, JP-T-2019-533737, JP-T-2020-507620, JP-T-2022-540302, etc., and commercially available materials such as the Alexa Fluor (registered trademark) series and the ATTO series can also be suitably used.
[0154]
[0155] In the polymer microparticles of the present invention, the light-emitting material or coloring material may contain other compounds as needed in addition to the compounds exemplified above. For example, an assist dopant may be contained to improve the efficiency of energy transfer from excitation light to the light-emitting material. Furthermore, if it is desired to add a luminescent color, the polymer microparticles may further contain the above-mentioned organic light-emitting material or a known light-emitting material such as an inorganic phosphor, a fluorescent pigment, a fluorescent dye, or quantum dots.
[0156] (Method for producing polymer microparticles) The method for producing polymer microparticles according to the embodiment of the present invention (hereinafter sometimes abbreviated as the method for producing polymer microparticles of the present invention) is not particularly limited as long as it can produce the above-mentioned polymer microparticles of the present invention. For example, the polymer microparticles of the present invention can be produced by known methods such as interfacial polymerization, W / O system submerged drying method, Stöber method, spray drying method, in situ polymerization method, phase separation method from aqueous solution, phase separation method from organic solvent, melt dispersion cooling method, and air suspension coating method.
[0157] Among the above-mentioned methods, a method of producing microparticles from a resin that has already been produced by polymerization or a composition containing the resin is preferred, from the viewpoint of being able to prevent emulsifiers, polymerization initiators, and their altered products from remaining in the polymer microparticles.
[0158] In particular, the method for producing polymer microparticles of the present invention preferably comprises the following steps (a) and (b), and is a method in which steps (a) and (b) are performed sequentially. Specifically, step (a) is a step of forming an emulsion containing two phases in its molecular structure: a first phase and a second phase, as described below. The first phase is a polymer phase containing a resin having at least one ring structure selected from the group consisting of an aliphatic hydrocarbon ring, an aliphatic heterocycle, and a ring containing an SP3 carbon, and an organic solvent. The second phase is a poor solvent phase containing a water-soluble polymer and at least one of water and an alcohol. Step (b) is a step of subjecting the emulsion obtained in step (a) to at least one of heating and reducing pressure under stirring to remove some or all of the organic solvent contained in the emulsion, thereby precipitating polymer microparticles.
[0159] This method involves removing the organic solvent from the homogeneous emulsion consisting of the first and second phases to extract polymer microparticles. Therefore, this method allows for the production of polymer microparticles with the desired sphericity and linseed oil absorption. Furthermore, by adjusting the viscosity ratio between the dispersed phase and the continuous phase, the interfacial tension, and the applied stirring power, polymer microparticles with the desired particle size and particle size distribution can be produced.
[0160] In one embodiment of the present method, in the above steps (a) and (b), the resin may be additionally crosslinked and cured at any stage, either in the emulsion state, during removal of the organic solvent, or in the fine particle state after removal of the organic solvent. This is preferable because the heat resistance of the resulting polymer fine particles is improved.
[0161] In another embodiment of the present method, it is preferable that the steps (a) and (b) do not include the polymerization step described above. In this case, impurities such as the polymerization initiator, catalyst, and unreacted monomers can be prevented from remaining in the resulting polymer microparticles, thereby suppressing changes in optical properties such as coloration caused by trace impurities.
[0162] From the viewpoint of suppressing changes in optical properties such as coloration caused by the above-mentioned trace impurities, the content of the polymerization initiator and its decomposition products in the polymer microparticles of the present invention is preferably less than 0.1 wt %, more preferably less than 0.05 wt %, even more preferably less than 0.01 wt %, and particularly preferably less than 0.001 wt %. The lower the content of the polymerization initiator and its decomposition products in the polymer microparticles, the better.
[0163] The organic solvent contained in the polymer phase is not particularly limited as long as it can dissolve the resin, which is the main component of the polymer microparticles, to form an organic phase and separate from the aqueous phase (the poor solvent phase in the emulsion) containing the water-soluble polymer and at least one of water and alcohol. Such organic solvents can be selected appropriately, but aprotic solvents are preferred. Specific examples of such organic solvents include hexane, cyclohexane, dioxane, toluene, diethyl ether, ethyl acetate, tetrahydrofuran, pyridine, ethylene glycol, acetonitrile, chloroform, and dichloromethane. Among these, hexane, cyclohexane, diethyl ether, ethyl acetate, tetrahydrofuran, acetonitrile, chloroform, and dichloromethane are more preferred because they have low boiling points and can selectively remove only the organic solvent in step (b). Furthermore, from the viewpoint of being less compatible with the poor solvent phase and being able to form a stable emulsion in the above step (a), hexane, cyclohexane, diethyl ether, ethyl acetate, chloroform, and dichloromethane are more preferred, and from the viewpoint of having excellent resin solubility, cyclohexane, ethyl acetate, chloroform, and dichloromethane are particularly preferred.
[0164] Furthermore, if the content of the solvent contained in the polymer microparticles of the present invention is excessively high, molecular motion of the resin in the polymer microparticles may be promoted, accelerating changes in the dispersion state of the luminescent material or colorant material. This may result in a deterioration in the durability of the polymer microparticles. In other words, to prevent a deterioration in the durability of the polymer microparticles, it is preferable to prevent residual solvent in the polymer microparticles, and the boiling point of the organic solvent is preferably 130°C or lower. The boiling point is more preferably 120°C or lower, even more preferably 100°C or lower, and particularly preferably 80°C or lower. Furthermore, the content of the solvent in the polymer microparticles is preferably less than 1 wt%, more preferably less than 0.5 wt%, and even more preferably less than 0.1 wt%.
[0165] In the method for producing polymer microparticles of the present invention, the water-soluble polymer preferably used is at least one selected from polyvinyl alcohol, poly(vinyl alcohol-ethylene) copolymer, polyethylene glycol, cellulose derivatives, and polyvinylpyrrolidones. Among these, polyvinyl alcohol, poly(vinyl alcohol-ethylene) copolymer, and polyethylene glycol are more preferred from the viewpoint of excellent interfacial stabilization effect between the dispersed phase and the continuous phase and the ability to form a homogeneous emulsion, and polyvinyl alcohol and polyethylene glycol are even more preferred from the viewpoint of high solubility in water and ease of removal by washing.
[0166] In the method for producing polymer microparticles of the present invention, the solvent that forms the poor solvent phase is not particularly limited as long as it dissolves the water-soluble polymer but does not dissolve the resin that is the main component of the polymer microparticles. For example, the solvent is at least one of water and alcohol. Examples of such solvents include water and alcohols such as methanol, ethanol, and isopropanol. Among these, water is preferred from the viewpoint of preventing the generation of voids in the shaped product due to the organic solvent.
[0167] Furthermore, in step (b), the emulsion obtained in step (a) is subjected to at least one of heating and decompression under stirring to remove some or all of the organic solvent contained in the emulsion. This results in the precipitation of polymer microparticles. The method for selectively removing only the organic solvent from the emulsion is not particularly limited. Specific examples of such methods include a method of monitoring the vapor temperature by observing the temperature of the liquid distilled at a desired degree of vacuum; a method of determining the vapor pressure from the solvent by observing the degree of vacuum and the temperature of the reaction vessel; and a method of collecting the distilled liquid and analyzing it by GC, NMR, or the like. In each of the above methods, the relationship between the temperature and vapor pressure of each solvent can be calculated using Antoine's equation (see, "Chemical Handbook, Basics II, Revised 3rd Edition," pp. 111-132, edited by the Chemical Society of Japan, Maruzen Co., Ltd."). Among these, the method of observing the vapor temperature is preferred from the viewpoint of being able to observe the volatilization behavior of the solvent.
[0168] The polymer microparticle solution thus obtained is separated into a solid such as polymer microparticles and a liquid such as a solution by a conventional solid-liquid separation method such as filtration, and the obtained solid (wet solid) is then washed with a solvent such as water, if necessary, and subjected to a drying step to obtain the desired dry powder (polymer microparticles).
[0169] (Composition and Optical Member) In one embodiment of the present invention, polymer microparticles can be mixed with a binder resin, a solvent, an additive, etc. to form a composition containing polymer microparticles. A composition according to an embodiment of the present invention (hereinafter sometimes abbreviated as the composition of the present invention) contains, for example, a binder resin and the polymer microparticles of the present invention and can be molded into a desired shape according to the member to which it is applied. For example, a desired optical member can be produced by molding a composition obtained by mixing polymer particles and a resin into a sheet, a lens, or other three-dimensional shape. That is, an optical member according to an embodiment of the present invention (hereinafter sometimes abbreviated as the optical member of the present invention) is a member containing the polymer microparticles of the present invention. The molding method of the composition is not particularly limited as long as it can be molded into the desired shape, but examples include a method of applying and drying using a known coating method, a molding method using an extruder, and a three-dimensional additive manufacturing method using a 3D printer, etc.
[0170] Representative structural examples of the optical member of the present invention include those shown in Figures 4 to 6. Figure 4 is a schematic cross-sectional view showing a first example of an optical member according to an embodiment of the present invention. Figure 5 is a schematic cross-sectional view showing a second example of an optical member according to an embodiment of the present invention. Figure 6 is a schematic cross-sectional view showing a third example of an optical member according to an embodiment of the present invention.
[0171] As shown in Fig. 4, the optical member 1A of the first example includes polymer fine particles 2a and a support 3a containing the polymer fine particles 2a. As shown in Fig. 4, the polymer fine particles 2a are dispersed inside the support 3a. The polymer fine particles 2a are an example of the polymer fine particles of the present invention. In the structural example shown in Fig. 4, the optical member 1A has a single-layer structure in which one type of polymer fine particles 2a is dispersed inside the single-layer support 3a.
[0172] As shown in Fig. 5, a second example optical element 1B includes two types of polymer microparticles 2a and 2b and a support 3a containing the two types of polymer microparticles 2a and 2b. As shown in Fig. 5, polymer microparticles 2a and polymer microparticles 2b are each dispersed within the support 3a. Both polymer microparticles 2a and polymer microparticles 2b are examples of polymer microparticles of the present invention. In the structural example shown in Fig. 5, the optical element 1B has a single-layer structure in which the two types of polymer microparticles 2a and polymer microparticles 2b are dispersed within the single-layer support 3a. These polymer microparticles 2a and polymer microparticles 2b have different optical properties, such as different emission colors.
[0173] As shown in Figure 6, the optical element 1C of the third example includes two types of polymer particles 2a and 2b and two layers of support 3a and 3b, each containing the two types of polymer particles 2a and 2b. Of these two support layers 3a and 3b, one type of polymer particles 2a is dispersed within the support 3a, and the other type of polymer particles 2b is dispersed within the support 3b. The polymer particles 2a and 2b are the same as those of the optical element 1B of the second example described above. In the structural example shown in Figure 6, the optical element 1C has a laminated structure including a single layer of support 3a containing dispersed polymer particles 2a and a single layer of support 3b containing dispersed polymer particles 2b different from the polymer particles 2a.
[0174] Here, the material of the support (for example, the supports 3a and 3b shown in FIGS. 4 to 6) is not particularly limited, and known metals, resins, glass, ceramics, paper, etc. can be used. However, from the viewpoints of transparency and processability, the support is preferably made of resin.
[0175] A first example of the optical member of the present invention is a color conversion member that converts incident light into light of a different wavelength. The polymer particles of the present invention containing a luminescent material have small optical loss and excellent durability, and therefore can be suitably used.
[0176] A second example of the optical member of the present invention is a color conversion substrate having a plurality of color conversion layers on a transparent substrate. In the present invention, the color conversion layer preferably includes a red conversion layer and a green conversion layer. The red conversion layer is formed of a phosphor material that absorbs at least blue light and emits red light. The green conversion layer is formed of a phosphor material that absorbs at least blue light and emits green light. Furthermore, partitions may be formed on the color conversion substrate, and the color conversion layer is preferably disposed between the partitions (in a recess). Such a color conversion substrate may be configured such that excitation light is incident from the transparent substrate side and the emitted color is visible from the side opposite the transparent substrate, or such that excitation light is incident from the color conversion layer side and the emitted color is visible from the transparent substrate side. The quantum yield of the color conversion layer is typically 0.5 or higher, preferably 0.7 or higher, more preferably 0.8 or higher, and even more preferably 0.9 or higher, when the color conversion substrate is irradiated with blue light having a peak wavelength of 440 nm or more and 460 nm or less.
[0177] (Light Source) The light source according to the embodiment of the present invention is not particularly limited, and in principle, any excitation light source can be used, such as a hot cathode tube, a cold cathode tube, a fluorescent light source such as an inorganic electroluminescence (EL), an organic EL element light source, an LED light source, an incandescent light source, or sunlight. Among these, an LED light source is a preferred light source. For example, in display and lighting applications, a light-emitting diode (LED light source) having a maximum emission wavelength in the range of 400 nm to 500 nm is a more preferred light source from the viewpoint of enhancing the color purity of blue light. Furthermore, as the light source, a blue LED light source having a maximum emission wavelength in the range of 430 nm to 480 nm is more preferred, and a blue LED light source having a maximum emission wavelength in the range of 450 nm to 470 nm is even more preferred.
[0178] The light source may have one emission peak or two or more emission peaks, but in order to improve color purity, it is preferable that the light source has one emission peak. It is also possible to use a combination of multiple light sources with different emission peaks.
[0179] (Light Source Unit) A light source unit according to an embodiment of the present invention (hereinafter sometimes abbreviated as the light source unit of the present invention) comprises the above-described light source and the polymer microparticles of the present invention or a member containing the polymer microparticles (for example, the composition of the present invention or an optical member, etc.). The light source unit of the present invention is useful for various light sources such as spatial illumination and backlighting. Specifically, the light source unit of the present invention can be used for applications such as displays, lighting devices, interiors, signs, and billboards, and is particularly suitable for use in displays and lighting devices.
[0180] (Display, lighting device) A display according to an embodiment of the present invention includes at least a light source unit including a light source and polymer fine particles as described above. For example, in a display such as a liquid crystal display, the light source unit described above is used as a backlight unit.
[0181] Furthermore, an illumination device according to an embodiment of the present invention includes at least a light source unit including a light source and polymer particles as described above. For example, this illumination device is configured to emit white light by combining a blue LED light source as the light source unit with polymer particles or a color conversion member containing the polymer particles that converts blue light from the blue LED light source into light with a longer wavelength.
[0182] (Ink) The polymer microparticles of the present invention can also be used in ink. An ink according to an embodiment of the present invention (hereinafter sometimes abbreviated as the ink of the present invention) is in a liquid, gel, or solid state containing at least the polymer microparticles of the present invention, and is used for writing characters or coloring surfaces. The polymer microparticles of the present invention have high sphericity and a uniform shape, and therefore, by applying them to the ink of the present invention, the smoothness of the printed surface using the ink can be improved and light scattering due to surface irregularities can be suppressed. Furthermore, since the polymer microparticles of the present invention also have excellent durability, by applying them to the ink of the present invention, printed materials using the ink can be used for a long period of time.
[0183] The present invention will be described below with reference to examples, but the present invention is not limited to the following examples. First, the measurement methods, evaluation methods, compounds, and resins used in the examples and comparative examples will be described.
[0184] [Compounds and Resins] In the following examples and comparative examples, compounds D-1 to D-5 were used as the luminescent material or coloring material contained in the polymer fine particles. Compounds D-1 to D-5 are the compounds shown below.
[0185]
[0186] In the following Examples and Comparative Examples, resins P-1 to P-7 were used as the resins that are the main components of the polymer particles. Resins P-1 to P-7 are the resins shown below. Resin P-1: Polymethyl methacrylate-hydrogenated styrene copolymer resin "Optimas" (registered trademark) 7500 (manufactured by Mitsubishi Gas Chemical Co., Ltd., Tg = 120°C, resin having a partial structure represented by general formula (1) and a partial structure represented by general formula (2)) Resin P-2: Polymethyl methacrylate-isobornyl methacrylate copolymer resin (Tg = 111°C) Resin P-3: Polymethyl methacrylate-cyclohexyl methacrylate copolymer resin (Tg = 94°C) Resin P-4: Polystyrene resin ("SIGMA-ALDRICH" (registered trademark), product number 331651, Tg = 100°C) Resin P-5: Polymethyl methacrylate resin BR-85 (manufactured by Mitsubishi Chemical Corporation, Tg = 105°C) Resin P-6: Polymethyl methacrylate-hydrogenated styrene copolymer resin (Tg = 120°C, resin having a partial structure represented by general formula (1) and a partial structure represented by general formula (2)) Resin P-7: Polymethyl methacrylate-hydrogenated styrene copolymer resin (Tg = 123°C, resin having a partial structure represented by general formula (1) and a partial structure represented by general formula (2))
[0187] Resin P-2 was synthesized by mixing methyl methacrylate and isobornyl methacrylate in a molar ratio of 85:15 and subjecting them to radical polymerization using azobisisobutyronitrile according to a known method. Resin P-3 was synthesized by mixing methyl methacrylate and cyclohexyl methacrylate in a molar ratio of 80:20 and subjecting them to radical polymerization in the same manner as for Resin P-2. After polymerization, Resins P-2 and P-3 were each purified by precipitation into methanol and thoroughly dried before use.
[0188] Resin P-6 and Resin P-7 were each synthesized by the following method. Specifically, methyl methacrylate and styrene were mixed in a molar ratio of 77:33, and methyl methacrylate and cyclohexyl methacrylate were mixed in a molar ratio of 32:68. Following a known method, a polymethyl methacrylate-styrene copolymer resin was obtained by radical polymerization using t-amylperoxy 2-ethylhexanoate. Subsequently, according to a known method, a hydrogenation reaction using Pd / C was carried out, thereby synthesizing Resin P-6 and Resin P-7, respectively. Each of the synthesized Resins P-6 and P-7 was subjected to adsorption and removal purification using spherical silica gel and activated carbon, followed by precipitation purification in methanol and thorough drying before use. 1 As a result of H-NMR measurement, the proportions of methyl methacrylate structural units in Resin P-6 and Resin P-7 were 75 mol % and 30 mol %, respectively. Furthermore, the hydrogenation reaction rates of the benzene ring moieties in Resin P-6 and Resin P-7 were both 99%.
[0189] [Measurement and Evaluation Method] (1) D50 particle size and D90 / D10 of polymer microparticles In this measurement and evaluation method, a dispersion of about 100 mg of polymer microparticles dispersed in about 5 mL of deionized water was added to a laser diffraction particle size distribution analyzer (Microtrac MT3300EX II) manufactured by Nikkiso Co., Ltd. until a measurable concentration was reached. The dispersion in this analyzer was subjected to ultrasonic dispersion at an output of 30 W for 60 seconds. Thereafter, the particle size at which the cumulative frequency from the small particle size side of the particle size distribution measured in 10 seconds is 50% was taken as the D50 particle size of the target polymer microparticles. In addition, the particle size at which the cumulative frequency from the small particle size side of the particle size distribution is 10% was taken as the D10 particle size, and the particle size at which the cumulative frequency is 90% was taken as the D90 particle size. The D90 / D10 of the target polymer microparticles was calculated from the ratio. The refractive index used during measurement was 1.52, and the refractive index of the medium (deionized water) was 1.333.
[0190] (2) Sphericity of polymer microparticles In this measurement and evaluation method, the sphericity of the polymer microparticles was calculated from the minor axis and major axis of each of the 30 polymer microparticles by observing 30 polymer microparticles randomly from a photograph taken with a scanning electron microscope (JSM-6301NF) manufactured by JEOL Ltd., according to the following formula:
[0191]
[0192] In the above formula, S is the sphericity of the polymer microparticles. a is the major axis of the polymer microparticles observed, and b is the minor axis of the polymer microparticles. n is the number of measurements of the polymer microparticles. In this measurement and evaluation method, the number of measurements was 30 (n=30).
[0193] (3) Linseed oil absorption of polymer microparticles In this measurement and evaluation method, in accordance with the Japanese Industrial Standards (JIS) JIS K 5101 (2004) "Pigment Test Method - Refined Linseed Oil Method," approximately 300 mg of polymer microparticles were precisely weighed on a watch glass, and refined linseed oil (manufactured by Kanto Chemical Co., Ltd.) was gradually added drop by drop using a burette, and these polymer microparticles and refined linseed oil were kneaded with a palette knife. After that, the series of operations from dropping the refined linseed oil to kneading was repeated until a sample mass was formed, and the point at which the paste of these polymer microparticles and refined linseed oil became smooth and hard was defined as the end point, and the linseed oil absorption of the target polymer microparticles (mL / 100 g) was calculated from the amount of refined linseed oil used for dropping.
[0194] (4) Light transmittance of resin In this measurement and evaluation method, a sample piece of resin with a film thickness of 20 μm or less was prepared, and the light transmittance of the sample piece was measured using a commercially available measuring instrument (for example, a violet-visible spectrophotometer (product name U-3010) manufactured by Hitachi, Ltd.). From the obtained measured values, the minimum value of the transmittance in the wavelength range of 400 nm to 800 nm was determined, and this minimum value was used as the measured value of the light transmittance of the target resin.
[0195] (5) Glass Transition Temperature of Resin In this measurement and evaluation method, the resin to be measured was heated in a nitrogen atmosphere using a differential scanning calorimeter (DSCQ20) manufactured by TA Instruments, at a rate of 20°C / min from 30°C to a temperature 30°C higher than the endothermic peak indicating the melting point of the resin. The DSC curve of the resin was obtained by heating the resin from 30°C to a temperature 30°C higher than the endothermic peak indicating the melting point of the resin at a rate of 20°C / min. The temperature at the point where the line equidistant along the vertical axis from the line extending the low-temperature and high-temperature baselines intersects with the curve representing the stepwise change in the glass transition was taken as the glass transition temperature of the resin. When the resin to be measured was an amorphous polymer that did not exhibit an endothermic peak at the melting point, the DSC curve of the resin was obtained by heating the resin from 30°C to 300°C. The mass of the resin required for measurement was approximately 8 mg.
[0196] (6) Molar absorption coefficient In this measurement and evaluation method, the compound to be measured is dissolved in a solvent (toluene for compounds D-1 to D-5) at 1 × 10 -5The compound was dissolved at a concentration of 1000 mol / L, and the absorption spectrum of the compound was measured using a U-3200 spectrophotometer (Hitachi, Ltd.) From the obtained absorption spectrum, the absorbance at the maximum absorption wavelength in the wavelength range of 300 nm or more was determined, and the molar absorption coefficient of the compound was calculated based on the obtained absorbance.
[0197] (7) Fluorescence Spectrum In this measurement and evaluation method, the compound whose fluorescence spectrum is to be measured is dissolved in a solvent (toluene for compounds D-1 to D-5) at 1 × 10 -6 The compound was dissolved at a concentration of 1000 mol / L, and the fluorescence spectrum of the compound was measured using a fluorescence spectrophotometer (Fluoromax 4, manufactured by Horiba, Ltd.) The half-width of the emission was determined from the obtained fluorescence spectrum.
[0198] (8) Luminescence Intensity of Polymer Microparticles In this measurement and evaluation method, polymer microparticles containing a luminescent material or a coloring material (hereinafter, these may be collectively referred to as "luminescent / coloring material") were sandwiched between cover glass plates, and the emission spectrum of the polymer microparticles was measured using a fluorescence spectrophotometer (Fluoromax 4, manufactured by Horiba, Ltd.) when excited with the maximum absorption wavelength of the luminescent / coloring material in a wavelength range of 300 nm or more. The widths of the slits on the excitation light side and the light-receiving side were fixed so that the intensity of the excitation light was the same. The luminescence intensity of the polymer microparticles to be evaluated was obtained from the emission spectrum measured as described above, and the obtained luminescence intensity was converted into a luminescence intensity relative to the luminescence intensity of the reference polymer microparticle (hereinafter referred to as relative luminescence intensity) for comparative evaluation. The evaluation results of the luminescence intensity of each polymer microparticle are shown in Tables 1 to 4 below. In Table 1, the relative luminescence intensity of the polymer microparticles is expressed as a relative value when the luminescence intensity of the polymer microparticles prepared in Example 1 is set to 100. In Table 2, the relative luminescence intensity of the polymer microparticles is expressed as a relative value when the luminescence intensity of the polymer microparticles prepared in Example 4 is set to 100. In Table 3, the relative luminescence intensity of the polymer microparticles is expressed as a relative value when the luminescence intensity of the polymer microparticles prepared in Example 8 is set to 100. In Table 4, the relative luminescence intensity of the polymer microparticles is expressed as a relative value when the luminescence intensity of the polymer microparticles prepared in Example 13 is set to 100.
[0199] (9) Durability of Polymer Microparticles In this measurement and evaluation method, a sample in which polymer microparticles were sandwiched between cover glass plates was placed on a surface light-emitting device equipped with a blue LED element (manufactured by ProLight; model number PM2B-3LBE-SD, emission peak wavelength: 460 nm), and a current of 10 mA was passed to turn on the blue LED element. The initial intensity of the light emitted from the polymer microparticles was measured using a spectroradiometer (CS-1000, manufactured by Konica Minolta). Then, a current of 200 mA was passed through the surface light-emitting device in an environment of 50 ° C. and 27% RH to turn on the blue LED element, thereby continuously irradiating light from the blue LED element, and the time until the emission intensity of the polymer microparticles decreased by 10% was observed. The obtained time was evaluated as the durability (light durability) of the polymer microparticles. However, the brightness was measured by removing the sample and the surface light-emitting device from the oven and allowing them to cool to room temperature.
[0200] (10) 1 In this measurement and evaluation method, 1 H-NMR was measured using a superconducting FTNMR EX-270 (manufactured by JEOL Ltd.) in a deuterated chloroform solution.
[0201] (11) Solvent content in polymer microparticles In this measurement and evaluation method, a sample was prepared by dissolving the target polymer microparticles (20 mg) in 2 mL of NMP or THF, and the solvent content in the sample was measured using a gas chromatograph (GC-2010) manufactured by Shimadzu Corporation under the following conditions. However, the solvent used to dissolve the polymer microparticles can be changed appropriately depending on the detection target. <Conditions> Detector: FID Column used: CP-Select 624 CB Detector temperature: 280°C Carrier gas: He Carrier gas flow rate: 6 mL / min Heating conditions: After holding at 40°C for 4 minutes, heat to 260°C at a heating rate of 8°C / min, and then hold for 16 minutes
[0202] (12) Content of polymerization initiator and its decomposition products in polymer microparticles In this measurement and evaluation method, a sample was prepared by dissolving the target polymer microparticles (20 mg) in 2 mL of NMP or THF, and the content of polymerization initiator and its decomposition products in the sample was measured using a gas chromatograph (GC-2010) manufactured by Shimadzu Corporation under the same conditions as those for measuring the solvent content described in (11) above. However, the solvent in which the polymer microparticles are dissolved can be changed appropriately depending on the target to be detected.
[0203] (13) Intrinsic Birefringence of Resin In this measurement and evaluation method, the dielectric polarization difference in each bond unit of the constituent units of the target resin was calculated by a molecular orbital method such as the AM1 method or PM3 method, and the intrinsic birefringence value was calculated as the volume average using the Lorentz-Lorentz equation below.
[0204]
[0205] In the above formula, Δn 0 : intrinsic birefringence value, ΔP: difference between the dielectric polarizability in the molecular chain axis direction and the dielectric polarizability in the direction perpendicular to the molecular chain axis, n: refractive index, d: density, N: Avogadro's number, M: molecular weight.
[0206] [Example 1] In Example 1, 45 g of resin P-1, the main component of the polymer microparticles, 21 mg of compound D-1 as the luminescent material, and 255 g of ethyl acetate as the solvent were mixed to prepare a 15 wt% polymer solution. Furthermore, 42 g of polyvinyl alcohol (GL-05, manufactured by Nippon Synthetic Chemical Industry Co., Ltd.) was dissolved in 258 g of water to prepare a 14 wt% aqueous polyvinyl alcohol solution. Next, the polymer solution and the aqueous polyvinyl alcohol solution were added to a 1 L tank, and the mixture was stirred at a temperature of 40 °C and a rotation speed of 300 rpm. This resulted in an emulsion in the 1 L tank. Next, the pressure in the 1 L tank was gradually reduced to 200 hPa using a diaphragm pump. After the pressure reached 200 hPa, the pressure was reduced for another hour to remove the organic solvent from the emulsion, thereby obtaining a polymer microparticle slurry.
[0207] Next, the solvent and the aqueous polyvinyl alcohol solution were removed from the polymer particle slurry by centrifugation and decantation of the supernatant. The polymer particle was then reslurried in water, washed with warm water at 80°C for 1 hour, and then filtered to remove impurities from the particles, yielding a polymer particle cake. The polymer particle cake was dried under reduced pressure, yielding the polymer particles of Example 1. The properties (particle properties) and material properties of the obtained polymer particles are as shown in Table 1. The obtained polymer particles were then placed on conductive tape and subjected to platinum vapor deposition, and the polymer particles were photographed at a magnification of 5000x using a scanning electron microscope (JSM-6301NF) manufactured by JEOL Ltd. A photograph of the polymer particles of Example 1 obtained in this manner is shown in FIG. 1.
[0208] In Example 2, polymer microparticles were prepared in the same manner as in Example 1, except that resin P-2 was used as the resin that was the main component of the polymer microparticles. The properties and material properties of the obtained polymer microparticles of Example 2 are as shown in Table 1.
[0209] In Example 3, polymer microparticles were prepared in the same manner as in Example 1, except that resin P-3 was used as the resin that was the main component of the polymer microparticles. The properties and material properties of the obtained polymer microparticles of Example 3 are as shown in Table 1.
[0210] [Comparative Example 1] In Comparative Example 1, 15 g of resin P-1 as the resin that is the main component of the polymer microparticles and 7.0 mg of compound D-1 as the luminescent material were melt-kneaded at 270°C using a micro-kneading extruder A300 (manufactured by Imoto Machinery Co., Ltd.) to obtain a kneaded product. The obtained kneaded product was molded into pellets and then freeze-pulverized using a freezer mill. In this way, the polymer microparticles of Comparative Example 1 were produced. The properties and material properties of the obtained polymer microparticles are as shown in Table 1. Furthermore, as in Example 1, the polymer microparticles of Comparative Example 1 were photographed at a magnification of 200x using a scanning electron microscope. A photograph of the obtained polymer microparticles of Comparative Example 1 is as shown in Figure 2.
[0211] Comparative Example 2 In Comparative Example 2, resin P-1 was used as the resin that is the main component of the polymer microparticles, and compound D-1 was used as the luminescent material. Resin P-1 (15 g), compound D-1 (7.0 mg), and toluene (60 g) were mixed as the solvent. This mixed solution was stirred and degassed at 300 rpm for 30 minutes using a planetary stirring and degassing device "Mazerustar KK-400" (manufactured by Kurabo Industries, Ltd.). This mixed solution was dried by spray drying to produce polymer microparticles of Comparative Example 2. The properties and material properties of the obtained polymer microparticles are as shown in Table 1. Furthermore, as in Example 1, the polymer microparticles of Comparative Example 2 were photographed at a magnification of 5000 times using a scanning electron microscope. A photograph of the obtained polymer microparticles of Comparative Example 2 is shown in FIG. 3.
[0212] In Comparative Example 3, polymer microparticles were prepared in the same manner as in Example 1, except that resin P-4 was used as the resin that was the main component of the polymer microparticles. The properties and material properties of the obtained polymer microparticles of Comparative Example 3 are as shown in Table 1.
[0213] In Comparative Example 4, polymer microparticles were prepared in the same manner as in Example 1, except that resin P-5 was used as the resin that was the main component of the polymer microparticles. The properties and material properties of the obtained polymer microparticles of Comparative Example 4 are as shown in Table 1.
[0214] [Examples 4 to 7] In Examples 4 to 7, polymer microparticles were prepared in the same manner as in Example 1, except that compounds D-2 to D-5 were used instead of compound D-1 as the luminescent material. However, the amount of luminescent material mixed was adjusted so that the amount of substance in the resulting polymer microparticles was the same. In each of Examples 4 to 7, even though the luminescent material mixed was different, polymer microparticles with high sphericity and smooth surfaces could be obtained, just like in Example 1. The properties and material characteristics of the obtained polymer microparticles are as shown in Table 2.
[0215] In Example 8, a polymer particle cake was obtained in the same manner as in Example 1, except that resin P-6 was used as the resin that was the main component of the polymer particles. The polymer particle cake was then dried under reduced pressure at a temperature of 50°C for 8 hours to obtain polymer particles of Example 8. The properties and material properties of the obtained polymer particles are as shown in Table 3.
[0216] In Example 9, polymer microparticles were prepared in the same manner as in Example 8, except that the drying conditions for the polymer microparticle cake were changed to 2 hours of reduced-pressure drying at a temperature of 50° C. The properties and material characteristics of the obtained polymer microparticles of Example 9 are as shown in Table 3.
[0217] In Example 10, polymer microparticles were prepared in the same manner as in Example 9, except that the solvent was changed to a mixed solvent of ethyl acetate and butyl acetate in a mixing ratio (ethyl acetate / butyl acetate) of 90 / 10. The properties and material properties of the obtained polymer microparticles of Example 10 are as shown in Table 3.
[0218] In Example 11, polymer microparticles were prepared in the same manner as in Example 8, except that 45 mg of azobisisobutyronitrile was mixed in addition to the resin, luminescent material, and solvent. The properties and material characteristics of the obtained polymer microparticles of Example 11 are as shown in Table 3.
[0219] [Example 12] In Example 12, polymer microparticles were prepared in the same manner as in Example 11, except that 80 mg of azobisisobutyronitrile was added. The properties and material properties of the obtained polymer microparticles of Example 12 are as shown in Table 3.
[0220] A comparison of Examples 8 to 12 reveals that the smaller the content of the solvent and the content of the polymerization initiator and its decomposition products in the polymer particles, the better the durability of the polymer particles.
[0221] [Example 13] In Example 13, polymer microparticles were prepared in the same manner as in Example 8, except that Compound D-2 was used instead of Compound D-1 as the light-emitting / coloring material. However, the amount of Compound D-2 mixed was adjusted so that the amount of substance in the resulting polymer microparticles would be the same. The properties and material properties of the obtained polymer microparticles of Example 13 are as shown in Table 4.
[0222] In Example 14, polymer microparticles were prepared in the same manner as in Example 13, except that resin P-7 was used as the resin that was the main component of the polymer microparticles. The properties and material properties of the obtained polymer microparticles of Example 14 are as shown in Table 4.
[0223] Comparing Example 13 and Example 14, it can be seen that even when resins having the same type of structural unit are used, a resin with a smaller magnitude of intrinsic birefringence results in smaller optical loss due to light diffusion and greater luminescence intensity.
[0224]
[0225]
[0226]
[0227]
[0228] Comparing Example 1 with Comparative Examples 1 and 2, it is clear that the polymer microparticles of Example 1, which have high sphericity, are superior to the polymer microparticles of Comparative Examples 1 and 2 in both relative luminescence intensity and durability.
[0229] Comparing Example 1 and Comparative Example 3, it can be seen that the polymer microparticles of Example 1, which use resin P-1, a resin having at least one ring structure selected from the group consisting of an aliphatic hydrocarbon ring, an aliphatic heterocycle, and a ring containing SP3 carbon in its molecular structure, have superior durability compared to the polymer microparticles of Comparative Example 3.
[0230] Furthermore, when comparing Examples 1 to 3, it can be seen that the polymer microparticles of Example 1, which use resin P-1, which corresponds to at least one of a resin having the above-mentioned ring structure in the polymer main chain and a resin in which the above-mentioned ring structure is directly linked to the polymer main chain, have particularly excellent durability.
[0231] As described above, the polymer microparticles, their production method, composition, optical member, light source unit, display and lighting device, and ink according to the present invention are suitable for achieving both improved durability and reduced optical loss.
[0232] 1A, 1B, 1C Optical member 2a, 2b Polymer fine particles 3a, 3b Support
Claims
1. Polymer microparticles containing a resin as a main component and containing a light-emitting material or a coloring material, characterized in that the polymer microparticles have a sphericity of 80 or more and 100 or less, and the resin has at least one ring structure selected from the group consisting of an aliphatic hydrocarbon ring, an aliphatic heterocycle, and a ring containing SP3 carbon in its molecular structure.
2. The polymer microparticles according to claim 1, characterized in that the polymer microparticles have a linseed oil absorption of 1 mL / 100 g or more and 200 mL / 100 g or less.
3. The polymer microparticles according to claim 1, characterized in that the ratio of D90 particle diameter to D10 particle diameter in the particle size distribution of the polymer microparticles, D9 particle diameter / D10 particle diameter, is 1 or more and 5 or less.
4. The polymer microparticles according to claim 1, characterized in that the content of the solvent in the polymer microparticles is less than 1 wt %.
5. The polymer microparticles according to claim 1, characterized in that the content of the polymerization initiator and its decomposition products in said polymer microparticles is less than 0.1 wt %.
6. The polymer microparticle according to claim 1, characterized in that the glass transition temperature of the resin is 100° C. or higher.
7. The polymer microparticles according to claim 1, characterized in that the resin is at least one of a resin having the ring structure in a polymer main chain and a resin in which the ring structure is directly linked to a polymer main chain.
8. The polymer microparticle according to claim 1, wherein the resin has a partial structure represented by general formula (1) and a partial structure represented by general formula (2) in its molecular structure. (In general formula (1), Y 1 and Y 2 may be the same or different, and each represents a hydrogen atom or an organic group having 1 to 20 carbon atoms. 3 ~Y 6 may be the same or different, and each represents a hydrogen atom or an organic group having 1 to 20 carbon atoms; and Y 3 ~Y 6 At least one of the groups is a group containing an aliphatic cyclic hydrocarbon structure.
9. Y in the above general formula (2) 3 ~Y 6 The polymer microparticle according to claim 8, wherein at least one of the groups is a substituted or unsubstituted cyclohexyl group.
10. Y in the above general formula (2) 3 ~Y 6 The polymer microparticle according to claim 8, wherein one of the groups is a substituted or unsubstituted cyclohexyl group, and the other three are hydrogen atoms.
11. The resin has a light transmittance of 85% or more in the wavelength range of 400 nm to 800 nm and an inherent birefringence of -30×10 -4 Above + 30 x 10 -4 2. The polymer microparticle of claim 1, wherein the polymer microparticle is a resin having a molecular weight of:
12. The polymer microparticles according to claim 1, wherein the light-emitting material or the coloring material is an organic pigment or an organic dye.
13. The luminescent material or the coloring material has a molar absorption coefficient of 10,000 M at a maximum absorption wavelength in a wavelength range of 300 nm or more. -1 ・cm -1 The polymer microparticle according to claim 1, characterized in that it contains at least one kind of organic material having the above properties.
14. The polymer microparticle according to claim 1, comprising at least one type of said luminescent material, the half-width of the emission spectrum of said luminescent material being 60 nm or less.
15. A composition comprising: a binder resin; and the polymer fine particles according to any one of claims 1 to 14.
16. An optical member comprising the polymer fine particles according to any one of claims 1 to 14.
17. A light source unit comprising: a light source; and the polymer microparticles according to any one of claims 1 to 14.
18. A display comprising a light source unit according to claim 17.
19. A lighting device comprising the light source unit according to claim 17.
20. An ink comprising the polymer fine particles according to any one of claims 1 to 14.
21. A method for producing polymer microparticles, comprising sequentially carrying out the following steps (a) and (b): step (a): forming an emulsion containing two phases: a polymer phase containing a resin having at least one ring structure selected from the group consisting of an aliphatic hydrocarbon ring, an aliphatic heterocycle, and a ring containing SP3 carbon in its molecular structure, and an organic solvent, and a poor solvent phase containing a water-soluble polymer, and at least one of water and an alcohol; and step (b): subjecting the emulsion to at least one of heating and reducing pressure while stirring to remove a part or all of the organic solvent contained in the emulsion, thereby precipitating polymer microparticles.
22. The method for producing polymer microparticles described in claim 21, characterized in that the water-soluble polymer is at least one selected from the group consisting of polyvinyl alcohol, poly(vinyl alcohol-ethylene) copolymers, polyethylene glycol, cellulose derivatives and polyvinylpyrrolidones.
23. The method for producing polymer microparticles according to claim 21, wherein the steps (a) and (b) do not include a polymerization step.
24. The method for producing polymer microparticles according to claim 21, characterized in that the resin is at least one of a resin having the ring structure in the polymer main chain and a resin in which the ring structure is directly linked to the polymer main chain.
25. The resin has a light transmittance of 85% or more in the wavelength range of 400 nm to 800 nm and an inherent birefringence of -30×10 -4 Above + 30 x 10 -4 The method for producing polymer microparticles according to claim 21, characterized in that the resin is one of the following:
Citation Information
Patent Citations
Spherical phosphor, sealing material for wavelength conversion type solar battery, solar battery module, and methods for producing them
JP2013087243A
Wavelength control optical member, light-emitting device, and lighting fixture
JP2017003815A
Flame-retardant polymer fine particles and method for producing the same
JP2020007529A
Polymer powder used in powder bed melt bonding method and method for producing three-dimensional molded object
JP2022001432A
Thermoplastic resin particle, and method for manufacturing three-dimensional object by powder bed fusion coupling system using the same
JP2022129658A