Stretch film
The stretch film with a styrene elastomer layer and an olefin resin surface layer addresses the challenges of stickiness and stretchability, achieving high elasticity and reduced hysteresis loss for improved handling and performance in various applications.
Patent Information
- Application Number
- PCT/JP2024/006828
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-02-26
- Publication Date
- 2024-10-03
AI Technical Summary
Existing stretch films with elastomers face challenges in achieving optimal stretchability and minimizing stickiness, particularly in thin films, which affects handling and performance in applications like sanitary and medical goods.
A stretch film with a styrene elastomer layer and a surface layer composed of an olefin resin and inorganic filler, where the surface layer is designed to reduce stickiness and enhance stretchability by controlling hysteresis loss and Shore A hardness, ensuring excellent elasticity and transportability.
The film achieves excellent stretchability with a hysteresis loss of less than 36%, providing improved handling and performance in applications requiring high elasticity and reduced stickiness, while maintaining dimensional stability and comfort.
Smart Images

Figure JP2024006828_03102024_PF_FP_ABST
Abstract
Description
Stretchable Film
[0001] The present invention relates to a stretch film.
[0002] Stretch films are used in a wide range of fields, including hygiene products, sporting goods, and medical products, to improve handling, wearing comfort (fit), etc. For example, they are used in garments such as underwear, waistbands of disposable diapers, side panels, leg gathers, incontinence products, sanitary napkins, bandages, surgical drapes, tightening bands, hats, swimming trunks, sports supports, medical supporters, and adhesive bandages.
[0003] Here, stretch films using stretchable elastomers have a strong stickiness due to the properties of the elastomer, which makes them difficult to handle, particularly in thin films.
[0004] Therefore, in order to prevent stickiness caused by the elastomer, a stretch film has been proposed that has a surface layer formed of a less sticky resin on the surface of the elastomer. More specifically, for example, a stretch film has been proposed that has an olefin-based resin layer laminated on at least one surface of the elastomer layer (see, for example, Patent Document 1).
[0005] JP 2016-112878 A
[0006] Generally, the elasticity of a film is evaluated by its permanent strain (the strain that remains after an external force is applied to the film and then removed), but there is a problem in that it is difficult to obtain an elastic film with elasticity approximating that of an ideal elastic body such as rubber by evaluation based solely on permanent strain.
[0007] Therefore, the present invention has been made in consideration of the above problems, and aims to provide an elastic film having a surface layer laminated on the surface of an elastomer layer, which has excellent elasticity.
[0008] In order to achieve the above object, the stretch film of the present invention is a stretch film comprising an elastomer layer and a surface layer laminated on at least one side of the elastomer layer, wherein the elastomer layer contains a styrene-based elastomer, and the surface layer is made of an olefin-based resin composition containing an olefin-based resin and an inorganic filler, and is characterized by having a hysteresis loss of less than 36% as described below.
[0009] (Hysteresis Loss) A strip-shaped test piece measuring 100 mm in one direction of the film and 25 mm in the direction perpendicular to that direction was cut from a stretch film, and this test piece was fixed to the grips of a testing machine so that the distance between the grips was 25 mm. The test piece was stretched in the longitudinal direction of the test piece at a speed of 254 mm / min so that the strain (elongation) calculated by the following formula (1) became 100%. The integrated area in the stress-strain curve (S-S curve) when this was done was defined as S1, and immediately after stretching, the test piece was contracted at the same speed until the load (N / 25 mm) on the test piece became 0. The integrated area in the stress-strain curve (S-S curve) when this was done was defined as S2, and the hysteresis loss [%] was calculated using the following formula (2).
[0010] Strain [%] = (L1 - L0) / L0 × 100 (1) Hysteresis loss [%] = S / S1 × 100 (2)
[0011] where L0 is the distance between the grippers (mm) before stretching, L1 is the distance between the grippers (mm) after stretching, S1 is the integrated area in the stress-strain curve when stretching from 0% to 100% strain, S2 is the integrated area in the stress-strain curve when shrinking from 100% strain to 0 stress, and S is the integrated area (S1-S2) in the stress-strain curve obtained by subtracting the integrated area S2 from the integrated area S1.
[0012] According to the present invention, it is possible to provide a stretchable film having a surface layer laminated on the surface of an elastomer layer, and having excellent stretchability.
[0013] FIG. 1 is a cross-sectional view showing a stretch film according to a first embodiment of the present invention. FIG. 2 is a plan view showing a stretch film according to the first embodiment of the present invention. FIG. 3 is a graph showing the integral area S1 in a stress-strain curve when stretched from 0% strain to 100%. FIG. 4 is a graph showing the integral area S2 in a stress-strain curve when contracted from 100% strain to 0 stress. FIG. 5 is a graph showing the integral area in a stress-strain curve obtained by subtracting the integral area S2 from the integral area S1. FIG. 6 is a cross-sectional view showing a stretch film according to a second embodiment of the present invention. FIG. 7 is a plan view showing a stretch film according to the second embodiment of the present invention.
[0014] The stretch film of the present invention will be specifically described below. Note that the present invention is not limited to the following embodiments, and can be appropriately modified and applied within the scope of the present invention.
[0015] [First embodiment] Fig. 1 is a cross-sectional view showing a stretch film according to this embodiment. As shown in Fig. 1, the stretch film 1 of this embodiment includes an elastomer layer 5 and surface layers 6 and 7 laminated on the surface of the elastomer layer 5.
[0016] (Elastomer Layer) The elastomer layer 5 is a layer that imparts stretchability to the stretch film 1, and this elastomer layer 5 contains a styrene-based elastomer, which is a thermoplastic elastomer.
[0017] Thermoplastic elastomer: The term "thermoplastic elastomer" refers to a polymer or polymer blend that has properties similar to vulcanized rubber at use temperatures, loses these properties at processing temperatures, can be easily processed, and regains its original properties when returned to use temperatures.
[0018] Furthermore, by using a styrene-based elastomer, the film is less likely to stretch, and the dimensional stability during transport is improved.
[0019] Examples of styrene-based elastomers used in the present invention include styrene-isoprene-styrene copolymers (SIS elastomers), styrene-isoprene block copolymers, styrene-butadiene-styrene block copolymers (SBS elastomers), styrene-butadiene block copolymers, hydrogenated styrene-isoprene-styrene block copolymers (styrene-ethylene-propylene-styrene block copolymers (SEPS elastomers)), hydrogenated styrene-butadiene-styrene block copolymers (styrene-ethylene-butylene-styrene block copolymers (SEBS elastomers)), and styrene-ethylene-ethylene-propylene-styrene copolymers (SEEPS elastomers). Among these, SIS elastomers are preferred because of their higher elasticity. Note that one type of styrene-based elastomer may be used alone, or two or more types may be used in combination.
[0020] Furthermore, thermoplastic elastomers are generally composed of hard segments that govern basic physical properties such as mechanical properties, and soft segments that govern elasticity, which is a rubber-like property. Examples of hard segments of styrene-based elastomers include polystyrene, and examples of soft segments of styrene-based elastomers include polybutadiene, polyisoprene, polyethylene, or hydrogenated products thereof.
[0021] When an SIS elastomer is used, the content of styrene units relative to the total units of the SIS elastomer is preferably 9% by mass or more and less than 50% by mass, and more preferably 12% by mass or more and less than 30% by mass. When the content of styrene units, which are hard segments, is 9% by mass or more, the stress at 10% elongation [N / mm 2 When the content of the soft segment is less than 50% by mass, the elasticity of the soft segment provides excellent stretchability in the direction perpendicular to the machine axis direction (hereinafter also referred to as "TD") shown in FIG. 2.
[0022] The Shore A hardness of the SIS elastomer is preferably 20 or more and less than 70. If the Shore A hardness is 20 or more, the stress at 10% elongation in the MD [N / mm 2 In addition, if the Shore A hardness is less than 70, the stretchability in the TD can be improved.
[0023] The "Shore A hardness" referred to here is measured using a type A durometer in accordance with JIS K 6253 at a temperature of 23°C.
[0024] When the SIS elastomer is used alone, the styrene unit content relative to the total units of the SIS elastomer (i.e., the entire elastomer layer) is preferably 30% by mass or less, more preferably 20% by mass or less. If the styrene unit content of the SIS elastomer is greater than 30% by mass, styrene has poor elasticity, which may increase the hysteresis loss described below and reduce the elasticity of the elastic film.
[0025] When the SIS elastomer is blended with other elastomers (for example, when SIS elastomers having different styrene unit contents are blended), the styrene unit content of the entire elastomer layer is preferably 9% by mass or more and 35% by mass or less. When the styrene unit content is 9% by mass or more, the stress at 10% elongation in the MD [N / mm 2 When the content is 35% by mass or less, the elasticity of the soft segment provides excellent stretchability in the TD.
[0026] When an SIS elastomer is used, the Shore A hardness of the entire elastomer layer is preferably 30 or more and less than 60. When the Shore A hardness is 30 or more, the stress at 10% elongation in the MD [N / mm 2 In addition, if the Shore A hardness is less than 60, the decrease in stretchability in the TD can be suppressed.
[0027] In addition, if the Shore A hardness of the entire elastomer layer is 30 or more, the stress at 10% elongation in the MD of the stretch film [N / mm2 ] is improved, and excellent conveying properties are obtained, but stretchability in the TD is reduced. In other words, since there is a trade-off between conveying properties in the MD and stretchability in the TD, the inventors have set the Shore A hardness of the entire elastomer layer to 30 or more, and have found that the stress at 10% elongation in the MD [N / mm 2 In order to improve the elasticity in the TD and to improve the reduced elasticity in the TD, the styrene unit content of the entire elastomer layer is set to 35% by mass or less.
[0028] The melt mass flow rate (MFR) of the styrene elastomer is preferably 0.5 to 22 g / 10 min, more preferably 3 to 15 g / 10 min. If the MFR of the styrene elastomer is greater than 22 g / 10 min, the melt viscosity may be too low, making it difficult to control the thickness during film molding. If the MFR of the styrene elastomer is less than 0.5 g / 10 min, melt fracture may occur during film molding, resulting in a rough film surface, or the high melt viscosity may cause the film to break during high-speed extrusion molding.
[0029] The melt mass flow rate can be measured in accordance with the standard of JIS K 7210.
[0030] The density of the styrene elastomer is 0.99 g / cm 3 The density of the styrene elastomer is preferably less than 0.99 g / cm 3 In the above cases, the stretchability of the film may decrease.
[0031] <Other Components> The elastomer layer 5 may contain components other than the styrene-based elastomer described above, as long as the effects of the present invention are not impaired. Examples of other components include resins other than styrene-based elastomers, such as olefin-based resins, amide-based antiblocking agents (e.g., stearic acid amide), plasticizers, UV absorbers, antioxidants, weather stabilizers, antistatic agents, colorants, antifogging agents, metal soaps, waxes, mildew inhibitors, antibacterial agents, nucleating agents, flame retardants, and lubricants. The other components may be added to the stretch film material as a masterbatch.
[0032] (Surface Layer) The surface layers 6 and 7 are layers that prevent stickiness of the elastomer layer 5 and suppress the occurrence of blocking in the stretch film 1. The surface layers are provided on at least one or both of the first and second surfaces of the elastomer layer, but from the viewpoint of sufficiently suppressing the occurrence of blocking in the stretch film 1, it is preferable that a surface layer be provided on both the first and second surfaces of the elastomer layer 5, as shown in Figure 1. Note that the surface layers 6 and 7 may be the same type of surface layer or different types of surface layers.
[0033] Each of the surface layers 6 and 7 is formed of an olefin-based resin composition containing an olefin-based resin and an inorganic filler. The surface layers 6 and 7 may also contain the other components described above, as necessary, within the range that does not impair the effects of the present invention.
[0034] <Olefin-based resin> Examples of the olefin-based resin include polyethylene-based resins and polypropylene-based resins. From the viewpoint of improving the stretchability of the surface layers 6, 7, polyethylene-based resins are preferred, and from the viewpoint of improving the heat resistance of the surface layers 6, 7, polypropylene-based resins are preferred.
[0035] For example, polyethylene resins include low-density polyethylene (LDPE) and linear low-density polyethylene (LLDPE). Among these, from the viewpoint of suppressing stickiness of the elastomer component, low-density polyethylene (density: 0.910 to 0.930 g / cm 3 ) is preferred, and from the viewpoint of improving stretchability, linear low-density polyethylene (density: 0.910 to 0.920 g / cm 3 ) is preferred.
[0036] Examples of polypropylene-based resins include homopolypropylene (H-PP) obtained by polymerizing propylene alone, random polypropylene (R-PP) obtained by copolymerizing propylene with ethylene, block polypropylene obtained by polymerizing homopolypropylene and then copolymerizing ethylene and propylene in the presence of the homopolypropylene (block polypropylene copolymerized with ethylene, B-PP), and propylene-based elastomers such as propylene-ethylene copolymers. Among these, random polypropylene (ethylene unit content: 5% by mass or less, melting point: 135 to 150°C) is preferred from the viewpoints of improving flexibility and improving heat resistance compared to polyethylene resins, since ethylene copolymerization reduces stereoregularity and decreases crystallinity. A propylene-based elastomer (propylene unit content: 70% by mass to 95% by mass, ethylene unit content: 5 to 30% by mass) is preferred from the viewpoint of improving stretchability.
[0037] The olefin resin may be used alone or in combination of two or more. For example, from the viewpoint of improving stretchability, a blend of random polypropylene and linear low-density polyethylene may be used. Furthermore, from the viewpoint of suppressing the occurrence of blocking in the elastomer component, a blend of propylene elastomer and low-density polyethylene may be used.
[0038] Furthermore, the content of the olefin-based resin in the entire surface layer 6 (or surface layer 7) (i.e., the entire olefin-based resin composition) is preferably 30% by mass or more and 85% by mass or less, when the entire surface layer is taken as 100% by mass. This is because, if the content of the olefin-based resin is less than 30% by mass, the content of the inorganic filler in the surface layer increases, which may result in a decrease in stretchability, and, if it is more than 85% by mass, the content of the inorganic filler in the surface layer decreases, which may result in blocking.
[0039] <Inorganic Filler> The inorganic filler is a component that imparts slipperiness to the surfaces of the surface layers 6 and 7 and further suppresses the occurrence of blocking in the stretch film 1 .
[0040] Examples of the inorganic filler include calcium carbonate, zeolite, silica, titanium oxide, calcium oxide, magnesium oxide, zinc oxide, clay, mica, barium sulfate, magnesium hydroxide, etc. The inorganic fillers may be used alone or in combination of two or more.
[0041] Furthermore, the content of the inorganic filler in the entire surface layer 6 (or surface layer 7) (i.e., the entire olefin-based resin composition) is preferably 15% by mass or more and 70% by mass or less, when the entire surface layer is taken as 100% by mass. This is because, if the content of the inorganic filler is less than 15% by mass, the content of the inorganic filler in the surface layer decreases, which may cause blocking, and, if it is more than 70% by mass, the content of the inorganic filler in the surface layer increases, which may cause a decrease in stretchability.
[0042] The average particle size of the inorganic filler is preferably 0.8 to 10 μm. If the average particle size of the inorganic filler is 0.8 μm or more, secondary aggregation of the inorganic filler is suppressed, dispersibility in the resin is improved, and slipperiness is improved. If the average particle size is 10 μm or less, the feel on the skin is improved.
[0043] <Method for Manufacturing Stretch Film> Next, a method for manufacturing the stretch film of this embodiment will be described in detail.
[0044] The stretch film of this embodiment is produced by molding a raw material containing the above-mentioned styrene-based elastomer, olefin-based resin, and inorganic filler into a film using an extruder.
[0045] More specifically, a styrene-based elastomer and, if necessary, the other components described above are mixed in a predetermined blending ratio to obtain a resin mixture for forming the elastomer layer. Then, an olefin-based resin, an inorganic filler, and, if necessary, other components are mixed in a predetermined blending ratio, and the mixture is extruded into strands using a co-rotating twin-screw extruder equipped with a strand die or the like, and cut to obtain pellets for forming the surface layer.
[0046] Next, using an extruder equipped with a T-die, the resin mixture for forming the elastomer layer and the pellets for forming the surface layer are extruded at a predetermined temperature, and a cast-fill process is used to obtain an unstretched raw film having an elastomer layer, a first surface layer (e.g., surface layer 6 in Figure 1 ) provided on a first surface of the elastomer layer, and a second surface layer (e.g., surface layer 7 in Figure 1 ) provided on a second surface of the elastomer layer.
[0047] The raw film is then stretched by uniaxial stretching to produce the stretch film 1 shown in Figures 1 and 2. The stretching method is not particularly limited, and examples include gear stretching, roll stretching, and tenter stretching.
[0048] For example, gear stretching can be performed using a pair of shaping rolls, each of which has a first shaping roll having a plurality of ridges extending circumferentially on the circumferential surface of a cylindrical roll body, and a second shaping roll having a plurality of ridges extending circumferentially on the circumferential surface of a cylindrical roll body, arranged opposite each other with a predetermined clearance provided so that the ridges of the first shaping roll mesh with the grooves between the ridges of the second shaping roll, and so that the grooves between the ridges of the first shaping roll mesh with the ridges of the second shaping roll.
[0049] Then, while the first shaping roll and the second shaping roll are rotated, the raw film before the above-mentioned gear stretching is passed between the first shaping roll and the second shaping roll, thereby forming a stretched region and an unstretched region between the convex ridges of the first shaping roll and the convex ridges of the second shaping roll.
[0050] In gear stretching, the stretching ratio can be adjusted by adjusting the width W of the apex of the ridges of the shaping roll, the height H of the ridges, the interval P between the apexes of adjacent ridges, the meshing depth D between the ridges of the first shaping roll and the ridges of the second shaping roll, etc. In addition, the stretching ratio in gear stretching can be easily calculated from the principle of stretching using Pythagoras' theorem.
[0051] The uniaxial stretching treatment described above refers to a stretching treatment carried out in either the MD or TD direction shown in Fig. 2. Note that a biaxial stretching treatment in which stretching treatment is carried out in both the MD and TD directions may also be carried out.
[0052] The stretching temperature in the uniaxial stretching treatment is usually room temperature (23±2°C). This is because stretching at room temperature can remove residual strain that remains during film molding and has the effect of reducing permanent strain. Stretching at a temperature higher than room temperature may increase orientation in the stretching direction, which may increase permanent strain.
[0053] The stretching ratio in the uniaxial stretching process is 1.5 times or more and 9 times or less. This is because if the stretching ratio is less than 1.5 times, residual strain remaining during film molding may not be removed. If the stretching ratio is greater than 9 times, the film may break when stretched. The "stretching ratio" referred to here refers to the multiple of the length of the stretched film in the stretching direction relative to the length of the film before stretching. In the case of gear stretching, it refers to the multiple of the length of the film in the stretched region relative to the length of the film before stretching. For example, if the distance between the apex of the convex stripes of the adjacent first shaping roll and the apex of the convex stripes of the second shaping roll (the width of the stretched portion of the film before gear stretching) is 1 mm and the meshing depth is √3 mm, the width of the stretched portion of the film will be 2 mm, and the stretching ratio will be 2 times.
[0054] The stretch film of this embodiment produced by the above-described method has a hysteresis loss of less than 36%, which makes it possible to prevent a decrease in the stretchability of the surface layers 6, 7 in the stretch film 1 having the surface layers 6, 7 laminated on the surface of the elastomer layer 5, and as a result, makes it possible to obtain a stretch film 1 with excellent stretchability. The hysteresis loss is preferably less than 30%, and more preferably less than 25%.
[0055] The "hysteresis loss" referred to here is calculated by the following method.
[0056] A strip-shaped test piece measuring 100 mm in one direction of the film and 25 mm in the direction perpendicular to that direction is cut from the stretch film, and this test piece is fixed to the grippers of a testing machine (e.g., Shimadzu Corporation, Autograph AG-5000A) so that the distance between the grippers is 25 mm. The test piece is then stretched in the longitudinal direction at a speed of 254 mm / min so that the strain (elongation) calculated by the following formula (1) is 100%. The integrated area in the stress-strain curve (S-S curve) when the test piece is stretched at the same speed immediately after stretching until the load (N / 25 mm) on the test piece becomes 0 is defined as S1. The integrated area in the stress-strain curve (S-S curve) when the test piece is contracted at the same speed immediately after stretching until the load (N / 25 mm) on the test piece becomes 0 is defined as S2. The hysteresis loss [%] is calculated using the following formula (2).
[0057] Strain [%] = (L1 - L0) / L0 × 100 (1) Hysteresis loss [%] = S / S1 × 100 (2)
[0058] where L0 is the distance between the grippers (mm) before stretching, L1 is the distance between the grippers (mm) after stretching, S1 is the integrated area in the stress-strain curve when stretching from 0% to 100% strain, S2 is the integrated area in the stress-strain curve when shrinking from 100% strain to 0 stress, and S is the integrated area in the stress-strain curve obtained by subtracting the integrated area S2 from the integrated area S1 (i.e., S = S1 - S2).
[0059] That is, the hysteresis loss can be calculated using the above formula (2) by subtracting the integrated area S2 in the stress-strain curve shown in FIG. 4 when the strain is contracted from 100% to 0 stress from the integrated area S1 in the stress-strain curve shown in FIG. 3 when the strain is extended from 0% to 100% (i.e., the integrated area S shown in FIG. 5) by the integrated area S1.
[0060] Furthermore, when the stretch film of this embodiment has a permanent set in the stretching direction of 7% or less, the plastic change is small, and therefore excellent stretchability can be obtained. The permanent set is preferably 6.5% or less.
[0061] The term "permanent strain" used herein refers to a value calculated by the following method.
[0062] A rectangular test piece measuring 100 mm in one direction of the film and 25 mm in the direction perpendicular to the one direction is cut from the stretch film, and this test piece is fixed to the gripping tools of a testing machine (e.g., Shimadzu Corporation, Autograph AG-5000A) so that the distance between the gripping tools is 25 mm. The test piece is then stretched in the longitudinal direction at a speed of 254 mm / min so that the strain (elongation) calculated by the following formula (1) becomes 100%, and then the test piece is immediately contracted at the same speed. The permanent set [%] is then calculated using the following formula (3).
[0063] Distortion [%] = (L1 - L0) / L0 x 100 (1) Permanent set [%] = (L2 - L0) / L0 x 100 (3)
[0064] where L0 is the distance (mm) between the grippers before stretching, L1 is the distance (mm) between the grippers after stretching, and L2 is the distance (mm) between the grippers when the load (N / 25 mm) on the test piece becomes 0 when contracting.
[0065] In addition, from the viewpoint of transportability of the stretchable film, the stress when stretching the stretchable film in the MD so that the strain (elongation) calculated by the above formula (1) becomes 10% (stress at 10% elongation) is 1.2 N / mm 2 It is preferable that the strength is 2N / mm or more. 2 More preferably, it is 3 N / mm or more. 2 More preferably, it is equal to or greater than this.
[0066] In addition, the stress when stretching the material in the TD so that the strain (elongation) calculated by the above formula (1) is 50% (stress at 50% elongation) is 0.5 to 1.5 N / mm 2 It is preferable that the strength is 0.8 to 1.2 N / mm 2 It is more preferable that the stress at 50% elongation is 0.5 N / mm 2 If the stress is too small, the film must be thickened to obtain appropriate stretchability, which may increase costs. 2In the case of a thickness exceeding 1000 mm, the stress is too great, so the film must be thin, and if it is too thin, handling may become difficult.
[0067] The thickness of the raw film is preferably 20 to 80 μm, more preferably 20 to 60 μm, and even more preferably 30 to 50 μm. If the thickness of the raw film is 20 μm or more, the stretchability is excellent. If the thickness of the raw film is 80 μm or less, the stretch film can be made thinner, resulting in lower rigidity and excellent stretchability.
[0068] The thickness of the elastomer layer 5 in the raw film is preferably 20 to 40 μm, more preferably 25 to 35 μm, and even more preferably 30 to 33 μm. If the thickness of the elastomer layer 5 is 20 μm or more, the stretchability of the stretch film 1 can be sufficiently obtained, and the film can be stably wound onto a roll during film formation. If the thickness of the elastomer layer 5 is 40 μm or less, the stretch film 1 can be made thinner, and the stress of the stretch film can be reduced.
[0069] Furthermore, the thickness of the surface layers 6, 7 in the raw film is preferably 1 to 10 μm, more preferably 1 to 5 μm, even more preferably 1 to 3 μm, and most preferably 1.2 to 2.2 μm. If the thickness of the surface layers 6, 7 is 1 μm or more, the occurrence of blocking in the stretchable film 1 after stretching can be sufficiently suppressed. If the thickness of the surface layers 6, 7 is 10 μm or less, the stretchability of the stretchable film 1 can be sufficiently obtained. Note that the surface layers 6, 7 may have the same thickness or different thicknesses.
[0070] Furthermore, from the viewpoint of improving the stretchability, even in the case of a stretch film 1 in which the thickness ratio of the surface layers 6, 7 to the entire stretch film is small, it is preferable that the thickness ratio of the surface layer 7 (or surface layer 8) to the elastomer layer 5 in the raw film (surface layer:elastomer layer) be 1:5 to 1:35, more preferably 1:8 to 1:30, and even more preferably 1:15 to 1:27.
[0071] Furthermore, the thickness of the stretchable film 1 after stretching is 85 to 95% of the original film when stretched at room temperature. In the case of gear stretching, the unstretched portion has the same thickness as the original film, and the stretched portion has 85 to 95% of the original film thickness.
[0072] By the above method, in this embodiment, excellent stretchability can be obtained in the stretch film 1 in which the surface layers 6 and 7 are laminated on the surface of the elastomer layer 5.
[0073] When the stretch film is multilayered, the compositions and thicknesses of the layers may be the same or different. When the stretch film is multilayered, the thickness refers to the total thickness of the multilayered film.
[0074] Second Embodiment Next, a second embodiment of the present invention will be described. Note that components similar to those in the first embodiment are given the same reference numerals and descriptions thereof will be omitted.
[0075] 6 is a cross-sectional view of a stretchable film according to this embodiment. As shown in FIG. 6, the stretchable film 20 according to this embodiment includes an elastomer layer 11 and surface layers 6 and 7 laminated on the surface of the elastomer layer 11.
[0076] (Elastomer layer) The elastomer layer 11 is a layer that imparts elasticity to the stretch film 1, and as shown in Figure 6, this elastomer layer 11 has a three-layer structure comprising a core layer 8 and intermediate layers 9 and 10 laminated on the surface of the core layer 8, with the intermediate layer 9 being provided between the core layer 8 and the surface layer 6, and the intermediate layer 10 being provided between the core layer 8 and the surface layer 7.
[0077] <Core Layer> The core layer 8 contains an olefin-based elastomer, which is a thermoplastic elastomer. The use of an olefin-based elastomer makes it possible to improve the stress at 50% elongation in the TD compared to the case where only the elastomer layer 5 containing a styrene-based elastomer is provided, as in the first embodiment.
[0078] The olefin-based elastomer used in the present invention may be a copolymer containing an olefin having 3 or more carbon atoms as the main component.
[0079] More specifically, examples of the elastomer include α-olefin copolymers such as propylene-ethylene copolymer, propylene-ethylene-1-butene copolymer, 1-butene-ethylene copolymer, 1-butene-propylene copolymer, 4-methylpentene-1-propylene copolymer, 4-methylpentene-1-1-butene copolymer, 4-methylpentene-1-propylene-1-butene copolymer, and propylene-1-butene copolymer. Elastomers in which the above-mentioned elastomers are dispersed in a crystalline polyolefin matrix may also be used. Among these, propylene-based elastomers (olefin-based elastomers whose hard segments are composed of polypropylene), such as propylene-ethylene copolymers, are preferred due to their higher stretchability. The olefin-based elastomers may be used alone or in combination of two or more.
[0080] Examples of the soft segment of the olefin-based elastomer include EPDM, EPM, EBM, IIR, hydrogenated styrene butadiene rubber (HSBR), NBR, and acrylic rubber (ACM).
[0081] Furthermore, when a propylene-based elastomer is used, the content of propylene units relative to all units of the propylene-based elastomer is preferably 70% by mass to 95% by mass, more preferably 80% by mass to 90% by mass. For example, in the case of a propylene-ethylene copolymer, the content of propylene units relative to all units is preferably 70% by mass to 95% by mass (i.e., the ethylene unit content is 5 to 30% by mass). If the content of propylene units, which are hard segments, is 70% by mass or more, strength is improved, resulting in excellent moldability, while if it is 95% by mass or less, excellent stretchability is obtained due to the elasticity of the soft segments.
[0082] The MFR of the propylene-based elastomer is preferably 0.5 to 10 g / 10 min, more preferably 2.0 to 8.0 g / 10 min. If the MFR of the propylene-based elastomer is greater than 10 g / 10 min, the melt viscosity may be too low, making it difficult to control the thickness during film molding. If the MFR of the propylene-based elastomer is less than 0.5 g / 10 min, melt fracture may occur during film molding, resulting in a rough film surface. If the MFR of the propylene-based elastomer is less than 2.0 g / 10 min, the melt viscosity may be so high that the film may break if extruded at high speed during film molding.
[0083] The density of the propylene elastomer is 0.900 g / cm 3 The density of the propylene-based elastomer is preferably less than 0.900 g / cm 3 In the above cases, the stretchability of the film may decrease.
[0084] Furthermore, the core layer 8 may contain components other than the propylene-based elastomer described above, provided that the effects of the present invention are not impaired. Examples of such components include resins other than the propylene-based elastomer, such as olefin-based resins, amide-based antiblocking agents (e.g., stearic acid amide), plasticizers, UV absorbers, antioxidants, weather stabilizers, antistatic agents, colorants, antifogging agents, metal soaps, waxes, mildew inhibitors, antibacterial agents, nucleating agents, flame retardants, and lubricants. These components may be added to the stretch film material as masterbatches.
[0085] <Intermediate Layer> As the intermediate layers 9 and 10, the same elastomer layer as the elastomer layer 5 described in the first embodiment (that is, the elastomer layer containing the styrene-based elastomer described above) can be used.
[0086] As mentioned above, when an SIS elastomer is blended with another SIS elastomer (for example, when SIS elastomers having different styrene unit contents are blended), the styrene unit content relative to the total units of the SIS elastomer is preferably 9% by mass or more and 35% by mass or less. However, when an SIS elastomer with a high styrene unit content (i.e., a styrene unit content of more than 30% by mass) is blended with an SIS elastomer with a low styrene unit content (i.e., a styrene unit content of 30% by mass or less), the blend ratio of the SIS elastomer with a high styrene unit content to the SIS elastomer with a low styrene unit content is preferably 20:80 to 50:50, from the viewpoint of improving stress in the MD while suppressing a decrease in stretchability in the TD. Within this blending ratio range, the stress at 10% elongation in the MD [N / mm 2 In order to improve the elasticity in the TD, which is sacrificed due to the Shore A hardness, the Shore A hardness can be increased to 30 or more, and in order to improve the elasticity in the TD, which is sacrificed due to the Shore A hardness, the styrene unit content of the entire elastomer layer can be reduced to 35 mass% or less.
[0087] <Method for Manufacturing Stretch Film> Next, a method for manufacturing the stretch film of this embodiment will be described in detail.
[0088] The stretch film of the present invention is produced by molding a raw material containing the above-mentioned olefin-based elastomer, styrene-based elastomer, olefin-based resin, and inorganic filler into a film using an extruder.
[0089] More specifically, an olefinic elastomer and, if necessary, the other components described above are mixed in a predetermined ratio to obtain a resin mixture for forming the core layer. Similarly, a styrene elastomer and, if necessary, the other components described above are mixed in a predetermined ratio to obtain a resin mixture for forming the intermediate layer. An olefinic resin, an inorganic filler, and, if necessary, the other components are mixed in a predetermined ratio, and the mixture is extruded into strands using a co-rotating twin-screw extruder equipped with a strand die, and then cut to obtain pellets for forming the surface layer.
[0090] Next, using an extruder equipped with a T-die, the resin mixture for forming the core layer, the resin mixture for forming the intermediate layer, and the pellets for forming the surface layer are extruded at a predetermined temperature, and a cast-fill process is used to obtain a raw film before stretching that has the core layer, an elastomer layer (e.g., elastomer layer 11 in Figure 6) having a first intermediate layer (e.g., intermediate layer 9 in Figure 6) provided on a first surface of the core layer and a second intermediate layer (e.g., intermediate layer 10 in Figure 6) provided on a second surface of the core layer, a first surface layer (e.g., surface layer 6 in Figure 6) provided on a first surface of the elastomer layer, and a second surface layer (e.g., surface layer 7 in Figure 6) provided on a second surface of the elastomer layer.
[0091] The raw film is then stretched uniaxially in either the MD or TD direction shown in Figure 7, thereby producing the stretchable film 20 shown in Figures 6 and 7. As with the first embodiment described above, the stretching method is not particularly limited, and examples include gear stretching, roll stretching, and tenter stretching. Biaxial stretching, in which stretching is performed in both the MD and TD directions, may also be performed.
[0092] Similarly to the first embodiment, the stretching temperature in the uniaxial stretching process is usually room temperature (23±2° C.), and the stretching ratio in the uniaxial stretching process is 1.5 times or more and 9 times or less.
[0093] The stretch film of this embodiment produced by the above-described method has a hysteresis loss of less than 36%, similar to the first embodiment described above, and therefore it is possible to prevent a decrease in the stretchability of the surface layers 6, 7 in the stretch film 20 having the surface layers 6, 7 laminated on the surface of the elastomer layer 11, and as a result, it is possible to obtain a stretch film 20 with excellent stretchability. The hysteresis loss is preferably less than 30%, and more preferably less than 25%.
[0094] Furthermore, the stretch film of this embodiment, like the first embodiment, has a permanent set of 7% or less in the stretching direction, making it possible to obtain excellent stretchability. The permanent set is preferably 6.5% or less.
[0095] In addition, similarly to the first embodiment described above, from the viewpoint of transportability of the stretchable film, the stress when stretching the stretchable film in the MD so that the strain (elongation) calculated by the above formula (1) becomes 10% (stress at 10% elongation) is 1.2 N / mm 2 It is preferable that the strength is 2N / mm or more. 2 More preferably, it is 3 N / mm or more. 2 More preferably, it is equal to or greater than this.
[0096] In addition, similarly to the first embodiment described above, from the viewpoint of suppressing an increase in cost, the stress when elongating the TD so that the strain (elongation) calculated by the above formula (1) becomes 50% (stress at 50% elongation) is 0.5 to 1.5 N / mm 2 It is preferable that the strength is 0.8 to 1.2 N / mm 2 It is more preferable that:
[0097] Similarly to the first embodiment, the thickness of the raw film is preferably 20 to 80 μm, more preferably 20 to 60 μm, and even more preferably 30 to 50 μm. The thickness of the elastomer layer 11 in the raw film is preferably 20 to 40 μm, more preferably 25 to 35 μm, and even more preferably 30 to 33 μm.
[0098] The thickness of the core layer 8 in the raw film is preferably 5 to 20 μm, more preferably 7 to 18 μm, and even more preferably 9 to 17 μm. The total thickness of the intermediate layers 9 and 10 in the raw film is preferably 10 to 25 μm, more preferably 12 to 22 μm, and even more preferably 14 to 20 μm.
[0099] In particular, in stretchable film 20 having a three-layer structure in which elastomer layer 11 is composed of core layer 8 and intermediate layers 9 and 10, from the viewpoint of improving the stress at 50% elongation in the TD while suppressing a decrease in stretchability in the TD, it is preferable that the thickness ratio of the core layer 8 in the raw film to the total thickness of intermediate layer 9 and intermediate layer 10 (core layer:total intermediate layer) be 20:80 to 50:50. In other words, there is a trade-off between improving the stress at 50% elongation in the TD and improving stretchability in the TD, and so long as the thickness ratio of the core layer thickness to the total thickness of the intermediate layers is within the above range, it is possible to achieve both an improvement in stress at 50% elongation in the TD and an improvement in stretchability in the TD.
[0100] Similarly to the first embodiment, the thickness of the surface layers 6, 7 in the raw film is preferably 1 to 10 μm, more preferably 1 to 5 μm, even more preferably 1 to 3 μm, and most preferably 1.2 to 2.2 μm.
[0101] Similarly to the first embodiment described above, the thickness ratio of the surface layer 7 (or surface layer 8) to the elastomer layer 11 in the raw film (surface layer:elastomer layer) is preferably 1:5 to 1:35, more preferably 1:8 to 1:30, and even more preferably 1:15 to 1:27.
[0102] As in the first embodiment, the thickness of the stretchable film 20 after stretching is 85 to 95% of the original film when stretched at room temperature. In the case of gear stretching, the unstretched portion has the same thickness as the original film, and the stretched portion has 85 to 95% of the original film thickness.
[0103] By the above method, in this embodiment, excellent stretchability can be obtained in the stretch film 20 in which the surface layers 6 and 7 are laminated on the surface of the elastomer layer 11.
[0104] When the stretch film is multilayered, the compositions and thicknesses of the layers may be the same or different. When the stretch film is multilayered, the thickness refers to the total thickness of the multilayered film.
[0105] The present invention will be described below based on examples. However, the present invention is not limited to these examples, and these examples can be modified or changed based on the spirit of the present invention, and such modifications are not excluded from the scope of the present invention.
[0106] The materials used to prepare the stretch film are as follows: (1) PP1: Random polypropylene (manufactured by Prime Polymer Co., Ltd., product name: F227, density: 0.90 g / cm 3 , MFR: 6.7 g / 10 min (230 ° C.)) (2) PP2: Random polypropylene (manufactured by Prime Polymer Co., Ltd., trade name: F327, density: 0.90 g / cm 3 , MFR: 7.0 g / 10 min (230 ° C.)) (3) PP3: Random polypropylene (manufactured by Prime Polymer Co., Ltd., trade name: F-744NP, density: 0.90 g / cm 3 , MFR: 7.0 g / 10 min (230 ° C.)) (4) PP4: Random polypropylene (manufactured by Prime Polymer Co., Ltd., trade name: 730NV, density: 0.90 g / cm 3 , MFR: 6.2 g / 10 min (230 ° C.)) (5) PP5: Random polypropylene (manufactured by Sumitomo Chemical Co., Ltd., trade name: FLX86E1, density: 0.89 g / cm 3 , MFR: 7.9 g / 10 min (230 ° C.)) (6) PP6: Random polypropylene (manufactured by SunAllomer Co., Ltd., trade name: PF621s, density: 0.90 g / cm 3 , MFR: 6.5 g / 10 min (230 ° C.)) (7) PP7: Random polypropylene (manufactured by SunAllomer Co., Ltd., trade name: PC630s, density: 0.90 g / cm 3, MFR: 7.5 g / 10 min (230 ° C.)) (8) PP8: Random polypropylene (manufactured by SunAllomer Co., Ltd., trade name: PC630a, density: 0.90 g / cm 3 , MFR: 7.5 g / 10 min (230 ° C.)) (9) Inorganic filler: calcium carbonate, average particle size: 1.8 μm (manufactured by Shiraishi Calcium Co., Ltd., trade name: PO-120B-10) (10) SIS elastomer 1 (manufactured by Nippon Zeon Co., Ltd., trade name: Quintac 3390, styrene unit content: 48 mass%, density: 0.98 g / cm 3 , Shore A hardness: 65, MFR: 14 g / 10 min (200 ° C.)) (11) SIS elastomer 2 (manufactured by Zeon Corporation, trade name: Quintac 3290, styrene unit content: 35 mass%, density: 0.93 g / cm 3 , Shore A hardness: 55, MFR: 10 g / 10 min (200 ° C.)) (12) SIS elastomer 3 (manufactured by Zeon Corporation, trade name: Quintac 3440, styrene unit content: 18 mass%, density: 0.93 g / cm 3 , Shore A hardness: 45, MFR: 10 g / 10 min (200 ° C.)) (13) SIS elastomer 4 (manufactured by Zeon Corporation, trade name: Quintac 3620, styrene unit content: 14 mass%, density: 0.93 g / cm 3 , Shore A hardness: 36, MFR: 9 g / 10 min (200 ° C.)) (14) SIS Elastomer 5 (manufactured by Zeon Corporation, trade name: Quintac 3433N, styrene unit content: 16 mass%, density: 0.93 g / cm 3 , Shore A hardness: 21, MFR: 12 g / 10 min (200 ° C.)) (15) SIS Elastomer 6 (manufactured by Kaneka Corporation, trade name: Shibstar 073T, styrene unit content: 30 mass%, density: 0.954 g / cm 3 , Shore A hardness: 45, MFR: 6 g / 10 min (230 ° C.)) (16) SIS elastomer 7 (manufactured by Kraton Corporation, trade name: Kraton D1161, styrene unit content: 15 mass%, density: 0.92 g / cm 3 , Shore A hardness: 32, MFR: 12 g / 10 min (200 ° C.)) (17) SIS elastomer 8 (manufactured by Kraton Corporation, trade name: Kraton D1126, styrene unit content: 21 mass%, density: 0.92 g / cm 3, Shore A hardness: 39, MFR: 22 g / 10 min (200 ° C.)) (18) Propylene-based elastomer (manufactured by ExxonMobil Corporation, trade name: Vistamax (registered trademark) 6102FL, polyethylene content: 16%, density: 0.862 g / cm 3 , Shore A hardness: 67, MFR: 3.0 g / 10 min (230 ° C.)) (19) Ethylene-based elastomer (manufactured by Dow Chemical Company, trade name: Infuse 9007, ethylene-octene copolymer, density: 0.864 / cm 3 , Shore A hardness: 64, MFR: 0.5 g / 10 min (190 ° C.)) (20) SBS elastomer (manufactured by Asahi Kasei Chemikels Corporation, trade name: Tufprene A, styrene unit content: 40 mass%, density: 0.95 g / cm 3 , Shore A hardness: 85, MFR: 2.6 g / 10 min (190 ° C.)) (21) SEBS elastomer (manufactured by Asahi Kasei Chemikels Corporation, trade name: Tuftec H1221, styrene unit content: 12 mass%, density: 0.89 g / cm 3 , Shore A hardness: 42, MFR: 4.5g / 10min (230°C))
[0107] (Example 1) <Preparation of Stretch Film> First, the materials shown in Table 1 were mixed to prepare a resin mixture for forming the elastomer layer and a resin mixture for forming the surface layer of Example 1 having the composition (parts by mass) shown in Table 1. Next, the resin mixture for forming the surface layer was extruded into a strand shape using a co-rotating twin-screw extruder (manufactured by JSW Corporation, product name: TEX28V-42CW-4V) equipped with a strand die under a condition of 200°C, and then cut to obtain pellets for forming the surface layer.
[0108] Next, using an extruder (manufactured by Labotec) equipped with a T-die, the resin mixture for forming the elastomer layer and the pellets for forming the surface layer were extruded at 200°C, and a film having an elastomer layer, a first surface layer provided on a first surface of the elastomer layer, and a second surface layer provided on a second surface of the elastomer layer was formed by a cast film process.The film was then taken up on a take-up roll to obtain a raw film before stretching having the thickness shown in Table 1.
[0109] Then, this raw film was subjected to gear stretching treatment (stretching ratio: 5 times) in the TD at room temperature (23°C ± 2°C) to produce a stretchable film.
[0110] <Calculation of styrene unit content (relative to total units of SIS elastomer) in elastomer layer> The styrene unit content [%] of the elastomer layer in the prepared stretch film was calculated. More specifically, in Example 1, 100 parts by mass of SIS elastomer 3 (styrene unit content: 18% by mass) was contained per 100 parts by mass of the elastomer layer, so the styrene unit content of the elastomer layer was 18 x (100 / 100) = 18% by mass. The results are shown in Table 1.
[0111] <Measurement of Shore A Hardness of Elastomer Layer> The Shore A hardness of the elastomer layer was measured using a type A durometer (spring type rubber hardness tester) at a temperature of 23° C. in accordance with JIS K 6253. The results are shown in Table 1.
[0112] Calculation of the styrene-based elastomer content in the entire stretch film The styrene-based elastomer content [%] in the entire stretch film was calculated. More specifically, in Example 1, 100 parts by mass of SIS elastomer 3 (styrene-based elastomer) was contained per 100 parts by mass of the elastomer layer, and the thickness of the elastomer layer was 28 μm relative to the overall thickness of the stretch film (35 μm). Therefore, the styrene-based elastomer content in the entire stretch film was (28 / 35) × 100 = 80% by mass. The results are shown in Table 1.
[0113] <Measurement of Hysteresis Loss> From the prepared stretch film, a rectangular test piece measuring 100 mm in one direction (TD) of the film and 25 mm in the direction perpendicular to that direction (MD) was cut, and this test piece was fixed to the grippers of a precision universal testing machine (Shimadzu Corporation, Autograph AG-5000A) so that the distance between the grippers was 25 mm. The integrated area in the stress-strain curve (S-S curve) when the test piece was stretched in the longitudinal direction at a speed of 254 mm / min so that the strain (elongation) calculated by the above formula (1) was 100% was defined as S1. After stretching, the test piece was immediately contracted at the same speed until the load (N / 25 mm) of the test piece became 0. The integrated area in the stress-strain curve (S-S curve) when the test piece was contracted at the same speed was defined as S2. The hysteresis loss [%] was calculated from the above formula (2). The results are shown in Table 1.
[0114] <Measurement of Permanent Set> A rectangular test piece measuring 100 mm in one direction (TD) of the film and 25 mm in the direction perpendicular to the one direction (MD) was cut from the prepared stretch film. This test piece was fixed to the grippers of a precision universal testing machine (Shimadzu Corporation, Autograph AG-5000A) with a distance between the grippers of 25 mm. The test piece was then stretched in the longitudinal direction at a rate of 254 mm / min so that the strain (elongation) calculated by the above formula (1) was 100%, and then immediately contracted at the same rate. The permanent set in the TD [%] was calculated using the above formula (3). The test was conducted at room temperature (23°C ± 2°C). The results are shown in Table 1.
[0115] <Measurement of stress at 10% elongation> A rectangular test piece measuring 100 mm in one direction (MD) of the film and 25 mm in the direction perpendicular to that direction (TD) was cut from the produced stretch film, and this test piece was fixed to the grippers of a precision universal testing machine (Shimadzu Corporation, Autograph AG-5000A) so that the distance between the grippers was 25 mm. Then, the test piece was elongated in the longitudinal direction at a speed of 254 mm / min so that the strain (elongation) calculated by the above formula (1) was 10%, and the stress at 10% elongation in the MD [N / mm 2 The results are shown in Table 1.
[0116] <Measurement of stress at 50% elongation> A rectangular test piece measuring 100 mm in the direction perpendicular to one direction of the film (TD) and 25 mm in one direction (MD) was cut from the prepared stretch film, and this test piece was fixed to the grippers of a precision universal testing machine (Shimadzu Corporation, Autograph AG-5000A) so that the distance between the grippers was 25 mm. Then, the test piece was elongated in the direction perpendicular to the longitudinal direction at a speed of 254 mm / min so that the strain (elongation) calculated by the above formula (1) was 50%, and the stress at 50% elongation in the TD [N / mm 2 The results are shown in Table 1.
[0117] Examples 2 to 9 Except for changing the composition (parts by mass) of the surface layer, the composition (parts by mass) of the elastomer layer, and the thickness ratio between the surface layer and the elastomer layer to the conditions shown in Table 1, raw films having the thicknesses shown in Table 1 were stretched in the same manner as in Example 1 described above to produce stretchable films.
[0118] The styrene unit content in the elastomer layer was calculated, the Shore A hardness of the elastomer layer was measured, the styrene elastomer content in the entire stretch film was calculated, and the hysteresis loss, permanent set, stress at 10% elongation, and stress at 50% elongation were measured in the same manner as in Example 1. The results are shown in Table 1.
[0119] (Example 10) <Preparation of Stretch Film> First, the materials shown in Table 2 were mixed to prepare a resin mixture for forming the elastomer layer (core layer), a resin mixture for forming the elastomer layer (intermediate layer), and a resin mixture for forming the surface layer of Example 10, each having the composition (parts by mass) shown in Table 2. Next, the resin mixture for forming the surface layer was extruded into a strand shape using a co-rotating twin-screw extruder (manufactured by JSW Corporation, product name: TEX28V-42CW-4V) equipped with a strand die under a condition of 200°C, and then cut to obtain pellets for forming the surface layer.
[0120] Next, using an extruder (manufactured by Labotec) equipped with a T-die, the resin mixture for forming the elastomer layer (core layer), the resin mixture for forming the elastomer layer (intermediate layer), and the pellets for forming the surface layer were extruded at 200°C, and a cast film process was used to form an elastomer layer having a core layer, a first intermediate layer provided on a first surface of the core layer, and a second intermediate layer provided on a second surface of the core layer, a first surface layer provided on the first surface of the elastomer layer, and a second surface layer provided on the second surface of the elastomer layer.The film was then taken up on a take-up roll to obtain a raw film before stretching having the thickness shown in Table 2.
[0121] Then, this raw film was subjected to gear stretching treatment (stretching ratio: 5 times) in the TD at room temperature (23°C ± 2°C) to produce a stretchable film.
[0122] The styrene unit content in the elastomer layer was calculated, the Shore A hardness of the elastomer layer was measured, the styrene elastomer content in the entire stretch film was calculated, and the hysteresis loss, permanent set, stress at 10% elongation, and stress at 50% elongation were measured in the same manner as in Example 1. The results are shown in Table 2.
[0123] <Calculation of Olefin-Based Elastomer Content in the Entire Stretch Film> The olefin-based elastomer content [%] in the entire stretch film was also calculated. More specifically, in Example 10, 100 parts by mass of propylene-based elastomer (olefin-based elastomer) was contained per 100 parts by mass of the core layer, and the thickness of the core layer was 15.54 μm relative to the overall thickness of the stretch film (35 μm). Therefore, the olefin-based elastomer content in the entire stretch film was (15.54 / 35) × 100 = 44.4% by mass. The results are shown in Table 2.
[0124] Examples 11 to 25 Except for changing the composition (parts by mass) of the surface layer, the composition (parts by mass) of the elastomer layer (core layer), the composition (parts by mass) of the elastomer layer (intermediate layer), and the thickness ratio between the surface layer and the elastomer layer to the conditions shown in Tables 2 to 3, raw films having the thicknesses shown in Tables 2 to 3 were stretched in the same manner as in Example 10 described above to produce stretchable films.
[0125] The styrene unit content of the elastomer layer was calculated, the Shore A hardness of the elastomer layer was measured, the styrene elastomer content of the entire stretch film was calculated, the hysteresis loss was measured, the permanent set was measured, the stress at 10% elongation was measured, and the stress at 50% elongation was measured, all in the same manner as in Example 1. The olefin elastomer content of the entire stretch film was calculated in the same manner as in Example 10. The results are shown in Tables 2 and 3.
[0126] Comparative Examples 1 to 13 Except for changing the composition (parts by mass) of the surface layer, the composition (parts by mass) of the elastomer layer, and the thickness ratio between the surface layer and the elastomer layer to the conditions shown in Table 4, raw films having the thicknesses shown in Table 4 were stretched in the same manner as in Example 1 described above to produce stretchable films.
[0127] The styrene unit content of the elastomer layer was calculated, the Shore A hardness of the elastomer layer was measured, the styrene elastomer content of the entire stretch film was calculated, the hysteresis loss was measured, the permanent set was measured, and the stress at 10% elongation and the stress at 50% elongation were measured in the same manner as in Example 1. Furthermore, in Comparative Examples 1 to 3, the olefin elastomer content of the entire stretch film was calculated in the same manner as in Example 10. The results are shown in Table 4.
[0128] Comparative Examples 14 to 25 Except for changing the composition (parts by mass) of the surface layer, the composition (parts by mass) of the elastomer layer (core layer), the composition (parts by mass) of the elastomer layer (intermediate layer), and the thickness ratio between the surface layer and the elastomer layer to the conditions shown in Table 5, raw films having the thicknesses shown in Table 5 were stretched in the same manner as in Example 10 described above to produce stretchable films.
[0129] The styrene unit content of the elastomer layer was calculated, the Shore A hardness of the elastomer layer was measured, the styrene elastomer content of the entire stretch film was calculated, and the hysteresis loss, permanent set, stress at 10% elongation, and stress at 50% elongation were measured in the same manner as in Example 1. Furthermore, in Comparative Examples 20 to 25, the olefin elastomer content of the entire stretch film was calculated in the same manner as in Example 10. The results are shown in Table 5.
[0130]
[0131]
[0132]
[0133]
[0134]
[0135] As shown in Tables 1 to 3, in the stretch films of Examples 1 to 25, the elastomer layer contains a styrene-based elastomer, and the hysteresis loss is less than 36%, so it is clear that the stretch films have excellent stretchability.
[0136] On the other hand, as shown in Table 4, the stretch films of Comparative Examples 1 to 3 have a single elastomer layer and contain an olefin-based elastomer (propylene-based elastomer, ethylene-based elastomer) but no SIS elastomer, and therefore exhibit poor stretchability (hysteresis loss of 36% or more).Furthermore, the stretch films of Comparative Examples 1 and 2 have a Shore A hardness of 60 or more, and therefore exhibit poor stretchability (hysteresis loss of 36% or more).
[0137] Furthermore, in the stretch films of Comparative Examples 4, 7, and 12 to 13, the styrene unit content relative to the entire elastomer layer was greater than 35% by mass, and the Shore A hardness was 60 or more, so it can be seen that the stretchability was poor (the hysteresis loss was 36% or more).
[0138] Furthermore, in the stretch film of Comparative Example 5, the SIS elastomer and the SEBS elastomer were poorly compatible, and the added SEBS component aggregated, resulting in the formation of numerous aggregates (foreign matter) in the film, resulting in poor stretchability (hysteresis loss of 36% or more).
[0139] Furthermore, in the stretch film of Comparative Example 6, the elastomer layer contains an SBS elastomer with a very high Shore A hardness, and the Shore A hardness of the elastomer layer is 60 or more, so it is clear that the stretchability is poor (the hysteresis loss is 36% or more).
[0140] Furthermore, in the stretch films of Comparative Examples 8 to 10 and 16 to 17, plastic deformation progressed significantly in the elastomer layers of SIS elastomer 7 and SIS elastomer 8, resulting in large permanent strain in the TD, and thus poor stretchability (hysteresis loss of 36% or more). One possible reason for this is that the high proportion of diblock components contained in the styrene-based elastomer reduced the restoring force after elongation.
[0141] Furthermore, in the stretch films of Comparative Examples 11, 14-15, and 18-19, the styrene unit content relative to the entire elastomer layer was greater than 35% by mass, and therefore the stretchability was poor (the hysteresis loss was 36% or more).
[0142] Furthermore, in the stretch films of Comparative Examples 20 to 21, the styrene unit content of SIS elastomer 1 and SIS elastomer 2 contained alone in the core layer of the elastomer layer is greater than 30% by mass, and therefore the stretchability is poor (the hysteresis loss is 36% or more).
[0143] In the stretch films of Comparative Examples 22 to 25, the intermediate layer of the elastomer layer contains 50% or more of SIS elastomer 1 and SIS elastomer 2, each having a styrene unit content of 30% by mass or more. In this case, when the ratio of the total thickness of the intermediate layer to the sum of the thickness of the core layer and the total thickness of the intermediate layer of the elastomer layer (i.e., the total thickness of the elastomer layer, 28 μm) is 50% or less, as in Comparative Examples 22 to 25, the stress at 50% elongation in the TD is improved, but the decrease in stretchability cannot be suppressed, resulting in poor stretchability (hysteresis loss of 36% or more). Furthermore, the stretch films of Comparative Examples 22 and 25 also have poor stretchability (hysteresis loss of 36% or more) because their Shore A hardness is 60 or more.
[0144] As described above, the present invention is suitable for stretch films used in, for example, garments such as underwear, waistbands of disposable diapers, side panels, leg gathers, incontinence products, sanitary napkins, bandages, surgical drapes, tightening bands, hats, swimming trunks, sports supports, medical supporters, adhesive bandages, etc.
[0145] REFERENCE SIGNS LIST 1 Stretch film 5 Elastomer layer 6, 7 Surface layer 8 Core layer 9, 10 Intermediate layer 11 Elastomer layer 20 Stretch film
Claims
1. A stretch film comprising an elastomer layer and a surface layer laminated on at least one side of the elastomer layer, wherein the elastomer layer contains a styrene-based elastomer, and the surface layer is made of an olefin-based resin composition containing an olefin-based resin and an inorganic filler, and wherein the stretch film has a hysteresis loss of less than 36% as described below. (Hysteresis loss) A rectangular test piece measuring 100 mm in one direction of the film and 25 mm in the direction perpendicular to the one direction is cut from a stretch film, and this test piece is fixed to the grips of a testing machine so that the distance between the grips is 25 mm. The test piece is stretched in the longitudinal direction of the test piece at a speed of 254 mm / min so that the strain (elongation) calculated by the following formula (1) is 100%. The integral area in the stress-strain curve (S-S curve) when the test piece is stretched at the same speed immediately after stretching until the load (N / 25 mm) of the test piece becomes 0 is defined as S1, and the integral area in the stress-strain curve (S-S curve) when the test piece is contracted at the same speed immediately after stretching until the load (N / 25 mm) of the test piece becomes 0 is defined as S2. The hysteresis loss [%] is calculated from the following formula (2). Strain [%] = (L1 - L0) / L0 x 100 (1) Hysteresis loss [%] = S / S1 x 100 (2) where L0 is the distance between the grippers before elongation (mm), L1 is the distance between the grippers after elongation (mm), S1 is the integrated area in the stress-strain curve when the strain is elongated from 0% to 100%, S2 is the integrated area in the stress-strain curve when the strain is contracted from 100% to 0 stress, and S is the integrated area in the stress-strain curve (S1 - S2) obtained by subtracting the integrated area S2 from the integrated area S1.
2. The stretch film according to claim 1, wherein the styrene-based elastomer is a styrene-isoprene-styrene copolymer (SIS elastomer).
3. The stretch film according to claim 2, characterized in that the elastomer layer comprises a core layer and an intermediate layer laminated on at least one surface of the core layer, the intermediate layer being provided between the core layer and the surface layer.
4. The stretch film according to claim 3, wherein the core layer is made of an olefin-based elastomer, and the intermediate layer is made of the styrene-isoprene-styrene copolymer (SIS elastomer).
5. The stretch film according to claim 4, wherein the olefin-based elastomer comprises a propylene-based elastomer.
6. The stretch film according to any one of claims 1 to 5, characterized in that the olefin-based resin is random polypropylene and the inorganic filler is calcium carbonate.
Citation Information
Patent Citations
Elastic laminate and article including the same, and elastic laminate elongation and article including the same
JP2016112878A
Elastic laminate and manufacturing method thereof
JP2020183119A
Stretchable film
JP2021123677A
Stretchable film
WO2016013577A1
Stretching material, stretchable member, and garment product
WO2017034030A1