Composition, shaping method and shaped article
The use of a resin powder with tailored thermal and physical characteristics addresses the issues of heat shrinkage and warpage in 3D printing, enhancing the mechanical and dimensional qualities of printed objects by maintaining surface integrity and fluidity.
Patent Information
- Application Number
- PCT/JP2024/006876
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-02-26
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional 3D printer modeling methods using powder bed fusion bonding face issues with heat shrinkage and warpage due to temperature differences, leading to defects and non-uniform powder spreading, which affects the dimensional accuracy and mechanical properties of the printed objects.
A composition of resin powder with specific thermal and physical properties, including a controlled endothermic energy curve, particle size, sphericity, and melt flow rate, is used to minimize warpage and improve fluidity, ensuring the production of objects with enhanced mechanical properties and dimensional accuracy.
The composition effectively reduces warpage and improves the mechanical properties and dimensional accuracy of 3D printed objects by maintaining the surface integrity of resin particles and preventing excessive shrinkage, resulting in a more reliable and precise modeling process.
Smart Images

Figure JP2024006876_03102024_PF_FP_ABST
Abstract
Description
Composition, molding method, and molded object
[0001] The present invention relates to a composition, a molding method, and a molded object.
[0002] A known modeling method for 3D printers is powder bed fusion (PBF), which uses a laser as a heat source to melt and bond flatly laid powder one layer at a time. Patent Document 1 discloses a styrene-based resin as a modeling powder for powder bed fusion.
[0003] JP 2019-130864 A
[0004] Conventional resin particles for modeling have the problem that after melting by laser irradiation, the model shrinks due to the temperature difference with the interior of the printer (usually 150°C), causing warping of the sintered film and preventing the model from achieving the desired dimensions. On the other hand, if the temperature inside the printer is raised to prevent the aforementioned thermal shrinkage, the surface of the resin particles melts and becomes sticky, which reduces the fluidity of the particles during the powder-laying process, making it difficult to obtain a uniform powder-laying surface and resulting in modeling problems. The present invention has been made in consideration of the above-mentioned problems, and aims to provide a composition that can produce models with excellent performance in a 3D printer modeling method using a laser as a heat source.
[0005] One aspect of the present invention is a composition. The composition includes a resin powder, and in a differential scanning calorimetry measurement of the resin powder, the temperature at the intersection of a baseline after melting and an endothermic energy curve before melting is defined as T 1 The endothermic peak temperature during melting is T 2 When [T 2 -T 1 ] is 38 to 70°C, and T 2 The composition of the above aspect may be an aggregate of particles containing two or more types of resins with different melting points. In a differential scanning calorimetry measurement of the resin powder, the exothermic peak temperature during crystallization is T 3 When 30°C≦[T 2 -T 3]. The resin powder may have a median particle size D50 (volume basis) of 30 to 150 μm. The resin powder may have an average sphericity of 0.70 to 0.98. The resin powder may have a loose packing ratio (bulk specific gravity / true specific gravity) of 25 to 60%. The resin powder may have a melt flow rate (MFR) at 230°C of 5 to 100 [g / 10 min]. Another aspect of the present invention is a molding method. The molding method includes a step of forming a solidified resin layer in a predetermined pattern using the composition of any of the above-mentioned aspects. Yet another aspect of the present invention is a shaped object. The shaped object is obtained using the composition of any of the above-mentioned aspects.
[0006] According to the present invention, it is possible to provide a technique relating to a composition that can produce a modeled object with excellent performance in a 3D printer modeling method using a laser as a heat source.
[0007] FIG. 1 is a diagram schematically showing an endothermic energy curve obtained when a resin powder is subjected to differential scanning calorimetry.
[0008] Hereinafter, embodiments of the present invention will be described in detail. In this specification, the expression "a to b" in the description of a range of values means that the range is from a to b, unless otherwise specified.
[0009] The composition according to the embodiment is for three-dimensional modeling. In other words, the composition according to the embodiment can be used as a resin powder for modeling in a so-called 3D printer. The composition according to the embodiment contains a resin powder.
[0010] 1 is a diagram showing a typical endothermic energy curve obtained by differential scanning calorimetry (DSC) of a resin powder (also referred to as resin powder). As shown in FIG. 1, in the endothermic energy curve obtained by differential scanning calorimetry of the resin powder, the temperature at the intersection of the baseline after melting and the endothermic energy curve before melting is referred to as T 1 The endothermic peak temperature during melting is T 2 Let's say.
[0011] In this embodiment, [T 2 -T 1] is 38 to 70°C, preferably 40 to 66°C, and more preferably 42 to 62°C. 2 -T 1 By setting the lower limit of [T] to the above value or more, the resin particles can be sufficiently melted at the temperature inside the printer, and warping of the shaped object can be reduced. 2 -T 1 By setting the upper limit of [ ] to the above value or less, the resin particles melt moderately, the surface does not become sticky, and the fluidity does not decrease, so the temperature inside the printer can be increased, and ultimately, warping of the molded object can be reduced.
[0012] T 2 is 130 to 300°C, preferably 135 to 250°C, and more preferably 140 to 200°C. 2 By setting the lower limit of T to the above value or more, the mechanical properties of the material itself can be improved, and in turn, the strength of the shaped object can be improved. 2 By setting the upper limit to the above value or less, the temperature change when cooling to room temperature after molding is not too large, so shrinkage of the resin material is suppressed and the dimensional accuracy of the molded product can be improved.
[0013] In the endothermic energy curve obtained by differential scanning calorimetry of the resin powder, the exothermic peak temperature during crystallization is designated as T 3 When 30°C≦[T 2 -T 3 It is preferable that [T 2 -T 3 By setting the lower limit of [ ] to the above value or higher, it is possible to prevent the temperature inside the printer from falling below the crystallization temperature of the resin, making it less likely for the resin to crystallize when it cools to the temperature inside the printer after laser irradiation, thereby suppressing shrinkage of the molded object and ultimately preventing warping.
[0014] The median particle size D50 (volume basis) of the resin powder is preferably 30 to 150 μm, more preferably 30 to 130 μm, and even more preferably 30 to 100 μm. The median particle size D50 (volume basis) of the resin powder can be measured using a laser diffraction particle size analyzer. By setting the lower limit of the D50 of the resin powder at or above the above value, the gaps between the resin particles are reduced, making it easier to obtain dense molded objects, thereby improving mechanical properties and suppressing warping. Furthermore, the resin particles are less likely to melt in the printer, increasing their fluidity, which allows for a smooth powder surface during powder application and improves the density of the molded object. On the other hand, by setting the upper limit of the D50 of the resin powder at or below the above value, the powder is less likely to get caught on the recoater used to spread the resin particles during powder application, thereby suppressing streaks on the powder surface. Furthermore, when irradiated with a laser, the resin particles are more likely to melt to their cores, making it easier to obtain dense objects, thereby improving mechanical properties and suppressing warping of the objects.
[0015] The average sphericity of the resin powder is preferably 0.70 to 0.98, more preferably 0.80 to 0.90, and even more preferably 0.85 to 0.90. By setting the lower limit of the average sphericity of the resin powder at or above the above value, the fluidity of the resin particles is increased, the powder surface becomes smooth when laid down, and the density of the molded object is improved, thereby improving the mechanical properties and suppressing warping of the molded object. On the other hand, by setting the upper limit of the average sphericity of the resin powder at or below the above value, the fluidity of the resin particles is prevented from becoming too high, and the resin particles are packed appropriately, optimizing the contact points between the powder particles. As a result, even at the edge of the laser-irradiated area, the powder particles in the unirradiated area do not fuse together, and a molded object with the desired dimensions can be obtained.
[0016] The loose filling rate (bulk specific gravity / true specific gravity) of the resin powder is preferably 25 to 60%, more preferably 30 to 57%, and even more preferably 35 to 55%. By setting the lower limit of the loose filling rate at or above the above value, the gaps between the resin particles are reduced, making it easier to obtain a dense structure, improving mechanical properties, and suppressing warping of the molded product. On the other hand, by setting the upper limit of the loose filling rate at or below the above value, the contact points between the resin particles can be appropriately controlled, and adhesion of the resin particles to each other in non-printed areas (non-laser irradiated areas) can be suppressed.
[0017] The melt flow rate (MFR) of the resin powder at 230°C is preferably 5 to 100 [g / 10 min], more preferably 8 to 90 [g / 10 min], and even more preferably 10 to 80 [g / 10 min]. By setting the lower limit of the MFR of the resin powder at or above the above value, the fluidity during melting is not too low, allowing the gaps between the resin particles to be filled, resulting in a dense molded object, which improves mechanical properties and reduces warping of the molded object. On the other hand, by setting the upper limit of the MFR of the resin powder at or below the above value, the fluidity during melting is prevented from becoming too high, and the unirradiated portion at the edge of the laser-irradiated portion remains unmelted, allowing a molded object of the desired dimensions to be obtained.
[0018] The resin constituting the resin powder is not particularly limited as long as it satisfies the above-mentioned temperature characteristics and physical properties, but examples thereof include thermoplastic resins. Examples of the thermoplastic resin include crystalline resins. The term "crystalline resin" refers to a resin that has a melting peak when measured in accordance with ISO 3146 (Method for Measuring Plastic Transition Temperature, JIS K7121). Examples of the crystalline resin include polymers such as polyolefins, polyamides, polyesters, polyethers, polyphenylene sulfide (PPS), liquid crystal polymers (LCPs), polyacetals (POMs), and polyimides. Examples of polyolefins include polyethylene and polypropylene. These may be used alone or in combination of two or more. Examples of polypropylene include homopolypropylene, random polypropylene, and block polypropylene. Examples of polyamides include polyamide 410 (PA410), polyamide 6 (PA6), polyamide 66 (PA66), polyamide 610 (PA610), polyamide 612 (PA612), polyamide 11 (PA11), and polyamide 12 (PA12); and semi-aromatic polyamide 4T (PA4T), polyamide MXD6 (PAMXD6), polyamide 6T (PA6T), polyamide 9T (PA9T), and polyamide 10T (PA10T). These may be used alone or in combination of two or more. Among these, PA9T is also known as polynonamethylene terephthalamide, and is composed of a nine-carbon diamine and a terephthalic acid monomer. It is generally referred to as semi-aromatic because the carboxylic acid side is aromatic. Furthermore, polyamides disclosed herein also include aramids, which are fully aromatic and are composed of p-phenylenediamine and a terephthalic acid monomer, in which the diamine side is also aromatic. Examples of polyester include polyethylene terephthalate (PET), polybutadiene terephthalate (PBT), and polylactic acid (PLA).Examples of polyethers include polyether ether ketone (PEEK), polyether ketone (PEK), polyether ketone ketone (PEKK), polyaryl ether ketone (PAEK), polyether ether ketone ketone (PEEKK), polyether ketone ether ketone ketone (PEKEKK), polyether sulfone, etc. From the viewpoints of economy, availability, and energy conservation, polyolefins are preferred, and polypropylene is particularly preferred.
[0019] The resin powder is preferably an aggregate of particles containing two or more resins with different melting points. This allows rigidity to be achieved by the high-melting-point resin with a relatively high melting point, while elongation can be achieved by the low-melting-point resin with a relatively low melting point. The combination of high-melting-point and low-melting-point resins is not particularly limited as long as the temperature characteristics and physical properties described above are satisfied. Examples include homopolypropylene and random polypropylene, two types of random polypropylene with different PE contents, and PPS and PA6. In addition to the thermoplastic resins described above, the resin powder may also contain resin powders made of amorphous resins, crystal nucleating agents, compatibilizers, plasticizers, antioxidants, stabilizers, color inhibitors, pigments, dyes, UV absorbers, release agents, lubricants, flame retardants, antistatic agents, inorganic fibers, organic fibers, inorganic particles, and organic particles. These may be used alone or in combination of two or more. These may be mixed with the thermoplastic resin described above and incorporated into the resin powder, or attached to the surface of the resin powder.
[0020] Examples of powdering methods for producing the resin powder of this embodiment include melt granulation, in which a resin composition melted near its melting point is fibrous and then cut; pulverization, in which a resin material composed of a resin composition is cut or destroyed by applying impact or shear; and a method in which a resin incompatible with a fusible matrix component is dispersed in the matrix component and then the matrix component is removed to produce resin particles. To improve powder application, it is preferable for the powder shape to be rounded, i.e., to have high sphericity. Therefore, to obtain powder with such a suitable shape, it is preferable to select a powdering method suitable for the thermoplastic resin contained in the resin powder for the powder additive manufacturing method of this embodiment. Furthermore, when powdering is performed by pulverization, a classification process is preferably performed after pulverization in order to remove elongated powder from the pulverized powder and increase sphericity. In this case, classification methods such as air classification and sieve classification are examples of classification methods.
[0021] The composition described above allows for the production of three-dimensional objects at temperatures inside a printer (e.g., 150°C) at which the surfaces of the resin particles do not melt and stickiness does not occur. Furthermore, the thermal shrinkage of the resin during the laser irradiation process is alleviated, reducing warping of the sintered film, making it possible to obtain objects with the desired dimensions.
[0022] (Modeling Method) The modeling method according to the embodiment includes a step of forming a solidified resin layer in a predetermined pattern using the composition described above. The steps of the modeling method are described below.
[0023] First, a thin layer is formed using the above-described composition. Specifically, the composition is supplied onto the modeling stage, and then the composition is spread evenly on the modeling stage using a recoater (blade or roll) to form a single thin layer. The thin layer is formed directly on the modeling stage, or is laminated on top of an already spread thin layer or an already formed sintered film. The thickness of the thin layer can be adjusted according to the thickness of the sintered film and the precision of the model to be produced. The thickness of the thin layer is usually about 0.01 to 0.3 mm.
[0024] Next, a laser is selectively irradiated onto the area of the laminated thin layers where a model is to be formed. The temperature inside the printer during laser irradiation is [T 2 -20] ° C to [T 2 The resin powder in the thin layer is fused and bonded by the laser irradiation to form a sintered film. The resin powder that is not irradiated with the laser is collected as surplus powder and may be reused as the collected powder.
[0025] Next, the modeling stage is lowered by an amount corresponding to the thickness of the sintered film obtained by the laser irradiation, and the thin layer formation and laser irradiation are repeated in sequence. By this method, a solidified resin layer (3D model) with a predetermined pattern is produced.
[0026] (Shaped object) The shaped object of this embodiment is obtained by the above-described shaping method using the above-described composition. The shaped object of this embodiment has highly excellent dimensional accuracy because the sintered film obtained by laser irradiation is less likely to warp.
[0027] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various other configurations can also be adopted.
[0028] EXAMPLES The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these.
[0029] Compositions (aggregates of resin powder) were prepared using the resin components and blending amounts shown in Table 1. The main resin and sub-resin components shown in Table 1 are general-purpose products.
[0030] (Differential Scanning Calorimetry) A differential scanning calorimeter (Seiko Electronics Co., Ltd., SSC-5200) was used. 2 Measurement was carried out while blowing gas. First, the temperature was raised from 10°C to 330°C at a rate of 5°C per minute, and then held at 330°C for 4 minutes. Next, the temperature was lowered from 330°C to 10°C at a rate of 5°C per minute. The endothermic peak temperature at the time of melting in the temperature rise curve was taken as T 2 Then, T 2 The calorific value at a temperature 30°C higher than the melting point is taken as the baseline, and the temperature at the intersection of this baseline and the temperature rise curve before melting is taken as T 1The exothermic peak during crystallization in the cooling curve was defined as T 3 The values obtained from the endothermic energy curve are shown in Table 1.
[0031] (Median particle size D50 measurement (volume basis)) The particle size distribution of the powder was measured using a laser diffraction particle size distribution analyzer (Malvern, Mastersizer 3000, wet dispersion unit Hydro MV). The median particle size D50, which accounts for 50% by volume of the detected particle size distribution, was determined. The obtained values are shown in Table 1.
[0032] (Mean sphericity measurement) Using a circularity measuring device (FPIA-3000S, manufactured by Sysmex), the projected area and contour length (perimeter) were measured from the projection diagram of the particles, and the sphericity was calculated using the following formula. This was calculated for 1,000 to 2,000 particles, and the average value of these values was taken as the average sphericity of the composition (resin powder). The obtained values are shown in Table 1. Sphericity = (perimeter of a circle having the same area as the projected area of a particle) / (length of the contour of the projection diagram of the particle)
[0033] (Loose filling rate measurement (bulk specific gravity / true specific gravity)) The loose density was measured using a bulk specific gravity meter (compliant with JIS Z-2504, manufactured by Kuramochi Scientific Instruments Manufacturing Co., Ltd.). The obtained loose density was divided by the true density (true specific gravity) of the resin to calculate the "loose filling rate" of the resin powder. The obtained values are shown in Table 1.
[0034] (MFR Measurement) The MFR of the resin powder was measured at 230° C. under a load of 2.16 kg in accordance with JIS K7210 Method A. The obtained values are shown in Table 1.
[0035] (Warpage Evaluation) A powder bed fusion type 3D printer (RaFaElII 150C-HT) manufactured by Aspect Inc. was used to measure the internal temperature of the printer [T 2A 30 mm square piece of the composition was irradiated with a laser at a temperature of -15°C to obtain a sintered film (test piece) for one layer. The obtained test piece was placed on a horizontal surface with the convex downward, and a taper gauge was inserted into the gap between the horizontal surface and the test piece. The height of the gap was taken as the amount of warpage, and the amount of warpage was evaluated according to the following criteria. [Evaluation Criteria] AA: Warpage is 0.05 mm or less A: Warpage is more than 0.05 mm and 0.1 mm or less B: Warpage is more than 0.1 mm and 0.2 mm or less C: Warpage is more than 0.2 mm and 0.3 mm or less D: Warpage is more than 0.3 mm AA to C were considered pass, and D was considered fail.
[0036] (Physical properties of molded object: Measurement of flexural modulus of molded object) A three-dimensional molded object (test piece) measuring 10 mm in width, 80 mm in length, and 4 mm in thickness was produced from each composition using a powder bed fusion 3D printer (RaFaElII 150C-HT) manufactured by Aspect Inc. The flexural modulus in the thickness direction of the three-dimensional molded object was measured using a Tensilon universal testing machine (TENSIRON TRG-1250) manufactured by A&D Co., Ltd. In accordance with JIS K7171 (2016), a three-point bending test was performed with a support distance of 64 mm and a test speed of 2 mm / min to determine the flexural modulus. The measurement temperature was room temperature (23 ° C), the number of measurements was n = 5, and the average value was calculated. [Evaluation Criteria] A: 1500 MPa or more B: 1200 or more and less than 1500 MPa C: 1000 or more and less than 1200 MPa D: Less than 1000 MPa A to C were considered pass, and D was considered fail.
[0037] (Tensile Strain Evaluation) A tensile test was conducted on the obtained three-dimensionally shaped object in accordance with ISO 527. The testing machine used was an AGS-5kN (manufactured by Shimadzu Corporation). The test speed in the tensile test was 5 mm / min. The tensile test was conducted five times, and the average of the measured maximum tensile stresses was taken as the tensile strength, and the average of the strains at the maximum tensile point was taken as the tensile strain. The tensile strength and tensile strain were evaluated based on the following evaluation criteria. The results are shown in Table 3. The strain is expressed as "(final length - initial length / initial length) x 100". [Evaluation Criteria] A: Tensile strain of 10% or more B: Tensile strain of 5% or more but less than 10% C: Tensile strain of 3% or more but less than 5% D: Tensile strain of less than 3% A to C were considered pass, and D was considered fail.
[0038] <Dimensional Accuracy> Each composition (resin powder for 3D modeling) was stored for one week in an environment of 27°C and 80% RH. Using the resin powder for 3D modeling after one week of storage, a 3D model was produced using a powder bed fusion 3D printer (RaFaElII 150C-HT) manufactured by Aspect Inc. The conditions for producing the 3D model were as follows: Average powder layer thickness: 0.1 mm Laser output: 10 watts or more and 150 watts or less Laser scanning space: 0.1 mm Bed temperature: 15°C lower than the melting point of the resin The 3D model for evaluating dimensional accuracy was a rectangular parallelepiped with a side length of 50 mm and an average thickness of 5 mm, and was produced based on CAD data. The difference between the CAD data of the 3D model and the length of each side of the actually produced 3D model was calculated, and the average value was used as the dimensional difference. The "dimensional accuracy" was evaluated based on the following evaluation criteria. [Evaluation criteria] A: Dimensional difference is 0.02 mm or less B: Dimensional difference is more than 0.02 mm and not more than 0.05 mm C: Dimensional difference is more than 0.05 mm and not more than 0.10 mm D: Dimensional difference is more than 0.10 mm and not more than 0.15 mm A to C were considered to be acceptable, and D was considered to be unacceptable.
[0039]
Claims
1. A resin powder is contained, and in an endothermic energy curve obtained by performing differential scanning calorimetry on the resin powder, the temperature at the intersection of the baseline after melting and the endothermic energy curve before melting is defined as T 1 The endothermic peak temperature during melting is T 2 When [T 2 -T 1 ] is 38 to 70°C, and T 2 is 130 to 300° C., and the composition is for use in three-dimensional modeling.
2. The composition according to claim 1, wherein the resin powder is an aggregate of particles containing two or more types of resins having different melting points.
3. In the endothermic energy curve obtained by performing differential scanning calorimetry on the resin powder, the exothermic peak temperature during crystallization is T 3 When 30° C.≦[T 2 -T 3 3. The composition according to claim 1 or 2, wherein 4. The composition according to claim 1 or 2, wherein the resin powder has a median particle size D50 (volume basis) of 30 to 150 μm.
5. The composition according to claim 1 or 2, wherein the resin powder has an average sphericity of 0.70 to 0.
98.
6. The composition according to claim 1 or 2, wherein the resin powder has a loose packing ratio (bulk specific gravity / true specific gravity) of 25 to 60%.
7. The composition according to claim 1 or 2, wherein the resin powder has a melt flow rate (MFR) at 230° C. of 5 to 100 [g / 10 min].
8. A method for modeling, comprising the step of forming a solidified resin layer in a predetermined pattern using the composition according to claim 1 or 2.
9. A shaped object obtained by using the composition according to claim 1 or 2.
Citation Information
Patent Citations
Three-dimensional molding material, three-dimensional molding filament, wound body of the filament, and three-dimensional molding cartridge
JP2019130864A
Resin powder for solid fabrication, device for manufacturing solid fabrication object, and method of manufacturing solid fabrication object
JP2018196984A
3D printing
JP2021519709A
Copolymer powder having polyamide blocks and polyether blocks
JP2022532376A
Powder for powder lamination molding and manufacturing method for same
WO2020138188A1