Thermally-stable perovskite solar cell with composite interface passivation layer constructed based on self-assembled discotic liquid crystal and preparation method of thermally-stable perovskite solar cell

Through the composite interface passivation layer of HAT5 and o-F-PEAI, the stability problem of perovskite solar cells under high temperature and light is solved, achieving higher conversion efficiency and long-term stability.

CN118742162APending Publication Date: 2024-10-01XIAN UNIV OF SCI & TECH
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410986221.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Perovskite solar cells have insufficient thermal and photostability under high temperatures and light, leading to interface and grain boundary degradation, affecting the long-term performance of the device.

Method used

The composite interface passivation layer is constructed by combining discotic liquid crystal molecules 2,3,6,7,10,11-hexahydroxytriphenylenebenzene (HAT5) and 2-fluorophenylethyl iodide (o-F-PEAI). The assembly forms an ordered columnar phase, inhibits the aggregation and migration of o-F-PEAI, and enhances the thermal stability of the device.

Benefits of technology

The thermal stability and photostability of perovskite solar cells are significantly improved, the conversion efficiency is increased from 23.36% to 25.02%, the filling factor and short-circuit current are also improved, and the device can still maintain an initial efficiency of 80.1% after high-temperature aging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118742162A_ABST
    Figure CN118742162A_ABST
Patent Text Reader

Abstract

The invention relates to the field of perovskite solar cells, in particular to a thermally stable perovskite solar cell with a composite interface passivation layer constructed based on self-assembled discotic liquid crystal and a preparation method of the thermally stable perovskite solar cell. The cell comprises a substrate, an electron transport layer, a perovskite absorption layer, the composite interface passivation layer, a hole transport layer and an electrode, and the electron transport layer, the perovskite absorption layer, the composite interface passivation layer, the hole transport layer and the electrode are sequentially arranged on the substrate. Wherein the composite interface passivation layer is formed by dissolving o-F-PEAI in isopropanol, adding HAT5 and chlorobenzene to prepare a surface passivation solution, and then coating. According to the invention, a strategy of carrying out surface passivation by combining o-F-PEAI and HAT5 is provided, so that the thermal stability and the light stability of the perovskite solar cell are improved. The triphenyl nucleus in the HAT5 promotes pi-pi stacking self-assembly, the interaction with o-F-PEAI is enhanced, an ordered columnar phase is formed, and hole extraction in the one-dimensional direction is promoted. The HAT5 repairs the structural defects of the interface layer, retains the layered structure, and inhibits ion migration after annealing. The crystallinity and pi-pi accumulation of the HAT5 can be enhanced by heating at 85 DEG C, and the thermal stability of the HAT5 is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of perovskite solar cells, and in particular to a thermally stable perovskite solar cell based on a self-assembled discotic liquid crystal to construct a composite interface passivation layer and a preparation method thereof. Background Art

[0002] The power conversion efficiency of single-junction perovskite solar cells (PSCs) has reached 26.9%, which is comparable to that of single-crystalline silicon solar cells. However, the stability of PSCs still does not meet the requirements for commercialization. Stability issues include humidity, oxygen, light, and heat. Although encapsulation methods can solve water and oxygen stability issues, light and thermal stability remain key challenges that require urgent improvement. Thermal stability issues stem from the degradation of perovskite interfaces and grain boundaries. Under external stress, such as continuous illumination and temperatures exceeding 85°C, defects and mobile ions tend to accumulate at grain boundaries and interfaces. Therefore, passivating surface defects and suppressing ion migration are key to achieving long-term stability of PSCs.

[0003] Various surface defect passivators, including Lewis acid-base pairs, ultrathin insulating materials, low-dimensional perovskites, inorganic molecules, polymers, and halides, are beneficial to improving the stability of PSCs. Among them, phenethylammonium iodide (PEAI) and its derivatives are commonly used surface passivators in PSCs. However, when dissolved in isopropanol, PEAI tends to form a dense passivation layer on the surface of the perovskite film, which in turn hinders the holes from the perovskite absorption layer from passing through the passivation layer to the hole transport layer, which greatly reduces the short-circuit current of the PSC. In addition, PEAI is sensitive to temperature, resulting in a decrease in the passivation effect of the device. These shortcomings limit the further application of PEAI in PSC interface passivation. Therefore, it is necessary to propose a new strategy to enhance the thermal stability and photostability of such PSC devices through interface modification. Summary of the invention

[0004] Traditional technology uses phenylethylamine iodide (PEAI) and its derivatives for perovskite solar cells. There is ion migration in the interface passivation, which makes the thermal stability of the PSC cell above 85°C easily affected, thereby affecting the overall performance of the cell. Based on this, the present invention proposes a strategy for constructing a composite interface passivation layer by combining discotic liquid crystal molecules 2,3,6,7,10,11-hexahydroxytriphenylenebenzene (HAT5) with 2-fluorophenylethyl iodide (oF-PEAI) for surface passivation of perovskite films. First, HAT5 has significant steric hindrance, which inhibits the aggregation of oF-PEAI on the surface of the perovskite film, thereby promoting hole transport; secondly, due to π-π stacking, HAT5 can self-assemble into an ordered columnar phase under heating at 85°C, thereby having a high conductivity (especially holes) in one-dimensional direction. Most importantly, HAT5 heated at 85°C can self-repair its structural defects, improve its orderliness and π-π stacking, and thus enhance the thermal stability of the device. The excellent thermal stability originates from the strong interaction between HAT5 and oF-PEAI, which inhibits the migration of oF-PEAI into the perovskite. This study highlights the synergistic effect of composite interface modification and the key role of maintaining carrier balance and inhibiting ion migration in enhancing device stability during PSC aging.

[0005] To achieve the above object, on the one hand, the present invention provides a method for preparing a thermally stable perovskite solar cell based on a composite interface passivation layer constructed by self-assembled discotic liquid crystals, which comprises the following steps:

[0006] S1. Select fluorine-doped tin oxide conductive glass or indium-doped tin oxide conductive glass as a glass substrate, and after cleaning and ultraviolet ozone treatment, generate an electron transport layer on the glass substrate by any method selected from chemical bath deposition, water bath deposition, spin coating, scraping, and screen printing;

[0007] S2, mixing PbI2, FAI and MACl in a mixed solvent of N,N-dimethylformamide and dimethyl sulfoxide to form a perovskite precursor solution, and then coating it on the surface of the electron transport layer, annealing, and forming a perovskite absorption layer;

[0008] S3, dissolving oF-PEAI in isopropanol, adding 2,3,6,7,10,11-hexahydroxytriphenylenebenzene and chlorobenzene to prepare a surface passivation solution, and then coating it on the surface of the perovskite absorption layer to form a composite interface passivation layer;

[0009] S4, generating a hole transport layer made of Spiro-OMeTAD on the composite interface passivation layer;

[0010] S5. Generating an electrode on the hole transport layer by evaporation to finally obtain a perovskite solar cell.

[0011] As a further preferred technical solution of the present invention, the material of the electron transport layer in step S1 is any one of TiO2, ZnO, and SnO2.

[0012] As a further preferred technical solution of the present invention, the preparation method when the material of the electron transport layer in step S1 is TiO2 is as follows:

[0013] First, fluorine-doped tin oxide glass is selected as a glass substrate, and ultrasonically cleaned in glass cleaning liquid, deionized water and ethanol for 15 to 30 minutes respectively, blown dry with nitrogen, and then treated with ultraviolet ozone for 10 to 15 minutes;

[0014] Then, the glass substrate was placed in a 0.15-0.2 mol / L TiCl4 aqueous solution at 60-70°C for 45-60 minutes, and then washed alternately with deionized water and ethanol for multiple times;

[0015] Finally, the glass substrate is annealed at 180-200° C. for 20-30 minutes and treated in ultraviolet ozone for 15-20 minutes, thereby preparing a TiO2 electron transport layer.

[0016] As a further preferred technical solution of the present invention, the method for forming the perovskite absorption layer in step S2 is as follows:

[0017] Firstly, N,N-dimethylformamide and dimethyl sulfoxide were used as a mixed solvent, and PbI2, FAI and MACl with a molar ratio of 1:1:0.375 were added into the mixed solvent to obtain a perovskite precursor solution;

[0018] Then, the perovskite precursor solution is dripped onto the electron transport layer, and the first stage of spin coating is performed at a rotation speed of 2500-3500 rpm for 5-15 seconds; the second stage of spin coating is performed at a rotation speed of 4500-5500 rpm for 20-50 seconds, and 600 μL of ether is dripped as an anti-solvent 15-20 seconds before the end of the second stage;

[0019] Finally, after the second stage of spin coating is completed, annealing treatment is performed at a temperature of 120 to 200°C and an annealing time of 10 to 30 minutes to form a perovskite absorption layer.

[0020] As a further preferred technical solution of the present invention, the purity of PbI2 is 99.999%, the purity of FAI is 99.9%, and the purity of MACl is 99.99%.

[0021] As a further preferred technical solution of the present invention, in step S3, the mass ratio of oF-PEAI to 2,3,6,7,10,11-hexahydroxytriphenylenebenzene is 2 to 3:1.

[0022] As a further preferred technical solution of the present invention, the method for forming the composite interface passivation layer in step S3 is as follows:

[0023] First, oF-PEAI was dissolved in isopropanol, and then 2,3,6,7,10,11-hexahydroxytriphenylenebenzene and chlorobenzene were added to form a surface passivation solution;

[0024] Then, the surface passivation solution is dripped onto the surface of the perovskite absorption layer, and the coating is performed by rotation at a rotation speed of 1500 to 2500 rpm for 20 to 50 seconds to passivate the top surface and obtain a composite interface passivation layer.

[0025] As a further preferred technical solution of the present invention, the method for forming the hole transport layer in step S4 is as follows:

[0026] First, Spiro-OMeTAD, Li-TFSI acetonitrile solution and 4-tert-butylpyridine were mixed and dissolved in chlorobenzene, stirred at room temperature for 10 to 12 hours, and filtered through a 0.40 to 0.50 μm filter to prepare a Spiro-OMeTAD solution;

[0027] The Spiro-OMeTAD solution is dropped onto the composite interface passivation layer for spin coating at a rotation speed of 4000-5000 rpm for 20-30 seconds to obtain a hole transport layer.

[0028] As a further preferred technical solution of the present invention, the electrode is Au, Ag, Al or Pt electrode with a thickness of 70-100 nm and an active area of ​​0.08-0.10 cm 2 .

[0029] As a further preferred technical solution of the present invention, the thickness of the perovskite absorption layer is 200-1200 nm; the thickness of the passivation layer is 5-50 nm; and the thickness of the hole transport layer is 20-300 nm.

[0030] According to another aspect of the present invention, the present invention also provides a perovskite solar cell, which is prepared by the above method.

[0031] Compared with the prior art, the present invention can achieve the following beneficial effects:

[0032] The present invention proposes a strategy of combining oF-PEAI with HAT5 for surface passivation to improve the thermal stability and photostability of perovskite solar cells. HAT5 has obvious steric hindrance, which can prevent the aggregation of oF-PEAI, thereby improving the hole extraction efficiency. The triphenyl core in HAT5 promotes π-π stacking self-assembly, enhances the interaction with oF-PEAI, forms an ordered columnar phase, and promotes hole extraction in one-dimensional direction. Under the action of heating at 85°C, HAT5 repairs the structural defects of the interface layer, retains the layered structure, and inhibits the migration of ions after annealing. Heating can enhance the crystallinity and π-π stacking of HAT5 and enhance its thermal stability.

[0033] Compared with the conventional perovskite solar cell without the introduction of HAT5, the present invention improves the conversion efficiency of the perovskite solar cell from 23.36% to 25.02%, and the fill factor (FF) is increased to 83.32%, and the short-circuit current (J SC ) increased to 25.78mA / cm 2 The perovskite solar cell of the present invention can still maintain 82.4% of its initial efficiency after 1008 hours of single light aging. After 1008 hours of heat aging at 85°C without packaging, the thermal stability of the device still maintains 80.1% of its initial efficiency, indicating that the thermal stability and light stability are significantly improved compared with the traditional ones.

[0034] In summary, the synergistic effect of the composite additive of oF-PEAI combined with HAT5 proposed in the present invention on interface modification plays a key role in maintaining carrier balance to enhance device stability during the aging process, and has important practical value and guiding significance for the industrialization of perovskite batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0036] Figure 1 : POM images of HAT5 (a) heated and (b) cooled to 85°C.

[0037] Figure 2 As shown in the figure: (a) FTIR spectra of HAT5 and oF-PEAI+HAT5 films; (b) tangent diagram of the two-dimensional GIWAXS data of oF-PEAI and oF-PEAI+HAT5 films in the out-of-plane direction; (c) schematic diagram of the superposition direction of oF-PEAI and (d) oF-PEAI+HAT5.

[0038] Figure 3: (a) JV curve of perovskite solar cell under reverse scanning, (b) external quantum efficiency (EQE) spectrum and integrated photocurrent of comparative example 1 device and embodiment 1 device; in the figure, Control is comparative example and Target is embodiment.

[0039] Figure 4 The figures are: (a) Arrhenius plot of characteristic transition frequency derived from admittance spectrum; (b) environmental stability and (c) photostability of devices of comparative example 1 and example 1; (d) SEM images of perovskite films of comparative example 1 and (e) example 1 after 100 days of thermal aging; (f) thermal stability at 85°C of devices of comparative example 1 and example 1; in the figure, Control is comparative example and Target is example.

[0040] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings in conjunction with the embodiments. DETAILED DESCRIPTION

[0041] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0042] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0043] The discotic liquid crystal 2,3,6,7,10,11-hexahydroxytriphenylenebenzene (HAT5) of the present invention can be prepared by the following method: 0.50 g of 2,3,6,7,10,11-hexahydroxytriphenylenebenzene, 1.75 g of n-pentane bromide, 0.05 g of tetrabutylammonium bromide and 1.92 g of potassium carbonate are added into a 100 mL single-necked flask, and then 30 mL of DMF solvent is added; the reaction is stopped after heating and stirring at 100° C. for 16 hours; the reaction solution is extracted, filtered and concentrated to obtain a crude product, and the crude product is purified and separated by column chromatography to obtain a white solid HAT5.

[0044] Example 1

[0045] A method for preparing a thermally stable perovskite solar cell with a composite interface passivation layer constructed based on self-assembled discotic liquid crystals is provided, which specifically comprises:

[0046] S1. Preparation of TiO2 electron transport layer:

[0047] First, fluorine-doped tin oxide glass was selected as a glass substrate, and ultrasonically cleaned in glass cleaning liquid, deionized water and ethanol for 30 minutes respectively, dried by nitrogen, and then treated by ultraviolet ozone for 15 minutes;

[0048] Then, the glass substrate was placed in a 0.2 mol / L TiCl4 aqueous solution at 70 °C for 60 min and then washed three times with deionized water and ethanol alternately;

[0049] Finally, the glass substrate was annealed at 200° C. for 30 minutes and treated in ultraviolet ozone for 20 minutes to improve wettability, thereby preparing a TiO2 electron transport layer on the glass substrate.

[0050] S2. Using the anti-solution method and ether as the anti-solvent, the perovskite absorption layer was prepared:

[0051] PbI2 (1.2 mmol, 553.2 mg), FAI (1.2 mmol, 206.3 mg) and MACl (0.42 mmol, 28.3 mg) were mixed in 1 mL of a mixed solvent (DMF:DMSO = 4:1) to obtain FAPbI3, and a perovskite precursor solution was obtained;

[0052] Then, the perovskite precursor solution was dripped onto the electron transport layer, and the first stage of spin coating was performed at a speed of 3000 rpm for 10 s. The second stage of spin coating was performed at a speed of 5000 rpm for 30 s, and 600 μL of ether was quickly dripped onto the surface as an anti-solvent 20 seconds before the end of the second stage.

[0053] Finally, after the second stage of spin coating is completed, annealing treatment is performed at a temperature of 150° C. and an annealing time of 15 minutes to form a perovskite absorption layer (also known as a perovskite film) on the electron transport layer with a thickness of 800 nm.

[0054] S3. Use HAT5 and oF-PEAI to construct a composite interface passivation layer:

[0055] First, 5.5 mg of 2-fluorophenethyl iodide (oF-PEAI) was dissolved in 1 mL of isopropanol, and then 2 mg of HAT5 and 200 μL of chlorobenzene were added and mixed to prepare a surface passivation solution;

[0056] Then, the surface passivation solution was dripped onto the surface of the perovskite absorption layer and spin-coated at a speed of 2000 rpm for 30 seconds to perform top surface passivation without heat treatment, forming a composite interface passivation layer with a thickness of 50 nm on the perovskite absorption layer;

[0057] S4. Preparation of Spiro-OMeTAD hole transport layer:

[0058] First, 90 mg of Spiro-OMeTAD, 22 μL of Li-TFSI solution (520 mg dissolved in 1 mL of acetonitrile), and 36 μL of 4-tert-butylpyridine were dissolved in 1 mL of CB, and the solution was stirred at room temperature for 12 h and then filtered through a 0.45 μm syringe filter to prepare a Spiro-OMeTAD solution;

[0059] The Spiro-OMeTAD solution was dropped onto the composite interface passivation layer for spin coating at a rotation speed of 5000 rpm for 30 seconds to form a hole transport layer on the composite interface passivation layer with a thickness of 100 nm.

[0060] S5: A gold film about 80 nm thick was evaporated on the hole transport layer Spiro-OMeTAD as an electrode with an active area of ​​0.09 cm 2 , and eventually form a perovskite solar cell.

[0061] Comparative Example 1

[0062] A method for preparing a thermally stable perovskite solar cell without constructing a composite interface passivation layer is provided. The method is used as a comparative experiment of Example 1, and the only difference from Example 1 is that no HAT5 discotic liquid crystal material and chlorobenzene are added to the configured surface passivation solution, and the rest is the same as Example 1.

[0063] The present invention proposes a strategy of using discotic liquid crystal molecules 2,3,6,7,10,11-hexahydroxytriphenylenebenzene (HAT5) combined with 2-fluorophenethyl iodide (oF-PEAI) to construct a composite interface passivation layer for surface passivation of perovskite films. The structure of HAT5 is composed of a triphenylene core surrounded by a long alkoxy chain. The aromatic core promotes self-assembly to form a columnar phase, and the typical core spacing is about This promotes strong π-π stacking inside HAT5. In contrast, the flexible alkoxy chains act as insulators to isolate the aromatic cores of adjacent columns, and these factors enhance the charge transport along the HAT5 column axis through a synergistic mechanism. In addition, the huge steric hindrance of HAT5 effectively prevents the aggregation of oF-PEAI, creating a pathway for hole transport. Therefore, when HAT5 undergoes a liquid crystal phase transition, it has the ability to self-repair defects and charge traps within the column, thereby improving its crystallinity and charge transfer efficiency.

[0064] The POM images of HAT5 were measured at a heating and cooling rate of 0.5°C / min using a Linkam THMS600 hot stage control unit on a LEICA DM2500P. Figure 1 a. Figure 1b is the polarizing microscope (POM) image of HAT5 during heating and cooling, which shows that HAT5 forms an ordered hexagonal columnar phase in the liquid crystal phase (D ho ), this columnar phase gives HAT5 a high charge conduction efficiency in one dimension, with the longitudinal conduction efficiency (along the molecular stacking direction) being 1000 times higher than the lateral conduction efficiency (across the molecular disk surface).

[0065] Subsequently, the interaction between HAT5 and oF-PEAI was studied. Based on the method for preparing the composite interface passivation layer in Example 1 above, HAT5 film and HAT5+oF-PEAI film were prepared, and Fourier transform infrared spectra (FTIR) were recorded on a Bruker EQUINX55 spectrometer. The results showed that Figure 2 a. It can be seen that after HAT5 was introduced into oF-PEAI, the characteristic peak of the benzene ring of HAT5 shifted by 9.64 cmμ1, indicating that there is a strong interaction between HAT5 and oF-PEAI. In addition, based on the above Example 1, the oF-PEAI film before and after the addition of HAT5 was tested by in-situ grazing incidence wide-angle x-ray scattering (GIWAXS) images, as shown in FIG. Figure 2 b shows that oF-PEAI initially exhibits a distinct edge-on orientation in the out-of-plane direction, which usually hinders charge transfer. The introduction of HAT5 suppresses this edge-on orientation, thereby improving carrier transport. Figure 2 c and Figure 2 d is the superposition direction of oF-PEAI before and after adding HAT5. It can be seen that HAT5 promotes a more favorable face-to-face orientation.

[0066] In order to further demonstrate the beneficial effects of the present invention, the photoelectric performance of the perovskite solar cells (hereinafter referred to as devices) prepared in Example 1 and Comparative Example 1 was tested, and the results are shown in Table 1. After passivation with HAT5+oF-PEAI in Example 1, the device conversion efficiency (PCE) was 25.02%, the fill factor (FF) was 83.32%, and the short-circuit current (J SC ) is 25.78 mA / cm 2 Compared with Comparative Example 1, the J SC (Δ=0.57mA / cm 2 ) and FF (Δ = 3.03%). The JV curves were captured at a rate of 100 mW / cm2 using a Keithley 2400 light source under AM 1.5G illumination. The JV curve test results of the perovskite solar cells prepared in Comparative Example 1 and Example 1 are shown in FIG. Figure 3a. In order to verify the reliability and authenticity of the perovskite solar cell current, an external quantum efficiency (EQE) test was performed. The external quantum efficiency (EQE) was recorded by the QTest Station2000ADI EQE measurement system (Crowntech Inc.). The results are shown in Figure 3 As shown in b. It can be seen that Example 1 exhibits higher EQE and larger integrated current (25.43 mA / cm 2 ), while the integrated current of comparative example 1 is only 24.99 mA / cm 2 , which is consistent with the trend observed in the JV curve test results. The above test results show that the performance of perovskite solar cells passivated with HAT5+oF-PEAI is better.

[0067] Table 1

[0068]

[0069] The stability of the devices in Comparative Example 1 and Example 1 is further evaluated below. First, the ion migration activation energy (E a ) test, such as Figure 4 As shown in a, the E of the perovskite film of Comparative Example 1 and Example 1 a The values ​​are 66meV and 146meV respectively. a The larger the value, the higher the ion migration barrier in the perovskite film, which effectively inhibits ion migration and is beneficial to improving device stability. In addition, ToF-SIMS testing shows that after aging for 624 hours at high temperature, the oF-PEAI on the surface of the device in Comparative Example 1 diffuses downward, which is not conducive to the stability of the device. The introduction of HAT5 in Example 1 achieves the inhibition of the diffusion behavior of oF-PEAI in the device.

[0070] Subsequently, the humidity, light and heating stability of the device at 85°C were tested before and after optimization. Figure 4 As shown in Figure b, in an environment with a relative humidity of about 30%, after 2664 hours of aging, the device of Comparative Example 1 only retained 68.6% of its initial PCE, while the device of Example 1 retained 91.3% of its initial PCE. Similarly, Figure 4 c shows that under a single sunlight exposure, the performance of the unencapsulated comparative example 1 device significantly decreased after 1008 hours, while the device of Example 1 retained 82.4% of its initial performance. In addition, the SEM image of the perovskite film after aging was examined and it was found that the surface of the perovskite film of comparative example 1 became rough, and low-dimensional phases and pores (such as Figure 4 d), while the surface of the perovskite film of Example 1 remained smooth and flat, the pores were significantly reduced, and the formation of low-dimensional phases was suppressed, indicating that the thermal stability was improved ( Figure 4e). Meanwhile, after aging at 85°C for 1008 hours, the device of Comparative Example 1 almost lost its PCE, while the device of Example 1 maintained 80.1% of its initial PCE ( Figure 4 f). It can be seen that the stability of the perovskite solar cell after HAT5+oF-PEAI synergistic surface passivation is better.

[0071] Finally, the FF and surface element ratio of the two devices of Comparative Example 1 and Example 1 were monitored during the aging process. After aging, the FF of the device of Comparative Example 1 decreased by 72%, while that of the device of Example 1 only decreased by 15%. This is because oF-PEAI is transformed into a low-dimensional phase after heating, the passivation effect is lost, and defect formation increases, resulting in a significant decrease in the hole extraction rate. On the contrary, the increase in the crystallinity of HAT5 and the decrease in the π-π stacking distance after heating at 85°C enhance its hole extraction ability and reduce the adverse effects of the failure of oF-PEAI. In addition, due to the escape of iodine under the action of heating at 85°C, the I / Pb ratio in the device of Comparative Example 1 gradually decreases with aging, accelerating the degradation of the perovskite, while the HAT5 introduced in Example 1 acts as an iodine scavenger, inhibiting iodine escape and maintaining the I / Pb ratio in the perovskite film.

[0072] In summary, the aging tests under the above three conditions show that the device of Example 1 has excellent stability. This is because the π-π stacking of HAT5 is enhanced after heating to 85°C, which reduces the decrease in hole mobility caused by aging defects, thereby balancing the electron and hole mobilities and promoting carrier separation.

[0073] Although specific embodiments of the present invention are described above, those skilled in the art should understand that these are merely examples and that various changes or modifications may be made to the embodiments without departing from the principles and essence of the present invention. The scope of protection of the present invention is limited only by the appended claims.

Claims

1. A method for preparing a thermally stable perovskite solar cell based on a composite interface passivation layer constructed by self-assembled discotic liquid crystals. It is characterized in that The following steps are involved: S1. Select fluorine-doped tin oxide conductive glass or indium-doped tin oxide conductive glass as a glass substrate, and after cleaning and ultraviolet ozone treatment, generate an electron transport layer on the glass substrate by any method selected from chemical bath deposition, water bath deposition, spin coating, scraping, and screen printing; S2, PbI 2 , FAI and MACl are added into a mixed solvent of N,N-dimethylformamide and dimethyl sulfoxide to prepare a perovskite precursor solution, which is then coated on the surface of the electron transport layer and annealed to form a perovskite absorption layer on the electron transport layer; S3, dissolving oF-PEAI in isopropanol, adding 2,3,6,7,10,11-hexahydroxytriphenylenebenzene and chlorobenzene to prepare a surface passivation solution, and then coating the solution on the surface of the perovskite absorption layer to form a composite interface passivation layer on the perovskite absorption layer; S4, generating a hole transport layer made of Spiro-OMeTAD on the composite interface passivation layer; S5. Generating an electrode on the hole transport layer by evaporation to finally obtain a perovskite solar cell.

2. The method for preparing a thermally stable perovskite solar cell based on a composite interface passivation layer constructed by self-assembled discotic liquid crystal according to claim 1, It is characterized in that The material of the electron transport layer in step S1 is TiO 2 、ZnO、SnO 2 Any one of.

3. The method for preparing a thermally stable perovskite solar cell based on a composite interface passivation layer constructed by self-assembled discotic liquid crystal according to claim 1, It is characterized in that The material of the electron transport layer in step S1 is TiO 2 The generation method is as follows: First, fluorine-doped tin oxide glass is selected as a glass substrate, and ultrasonically cleaned in glass cleaning liquid, deionized water and ethanol for 15 to 30 minutes respectively, blown dry with nitrogen, and then treated with ultraviolet ozone for 10 to 15 minutes; Then, the glass substrate was placed in a 60-70°C, 0.15-0.2 mol / L TiCl 4 aqueous solution for 45 to 60 minutes, and then washed several times with deionized water and ethanol alternately; Finally, the glass substrate was annealed at 180-200°C for 20-30 minutes and treated in ultraviolet ozone for 15-30 minutes to prepare TiO 2 Electron transport layer.

4. The method for preparing a thermally stable perovskite solar cell based on a composite interface passivation layer constructed by self-assembled discotic liquid crystal according to claim 1, It is characterized in that The method for forming the perovskite absorption layer in step S2 is as follows: First, N,N-dimethylformamide and dimethyl sulfoxide were used as a mixed solvent to prepare PbI with a molar ratio of 1:1:0.

375. 2 , FAI and MACl are added into a mixed solvent to obtain a perovskite precursor solution; Then, the perovskite precursor solution is dripped onto the electron transport layer, and the first stage of spin coating is performed at a rotation speed of 2500-3500 rpm for 5-15 seconds; the second stage of spin coating is performed at a rotation speed of 4500-5500 rpm for 20-50 seconds, and 500-600 μL of ether is dripped as an anti-solvent 15-20 seconds before the end of the second stage; Finally, after the second stage of spin coating is completed, annealing treatment is performed at a temperature of 120 to 200°C and an annealing time of 10 to 30 minutes to form a perovskite absorption layer.

5. The method for preparing a thermally stable perovskite solar cell based on a composite interface passivation layer constructed by self-assembled discotic liquid crystal according to claim 4, It is characterized in that The PbI 2 The purity of is 99.999%, the purity of FAI is 99.9%, and the purity of MACl is 99.99%.

6. The method for preparing a thermally stable perovskite solar cell based on a composite interface passivation layer constructed by self-assembled discotic liquid crystal according to claim 1, It is characterized in that In step S3, the mass ratio of oF-PEAI to 2,3,6,7,10,11-hexahydroxytriphenylenebenzene is 2 to 3:

1.

7. The method for preparing a thermally stable perovskite solar cell based on a composite interface passivation layer constructed by self-assembled discotic liquid crystal according to claim 1, It is characterized in that The method for generating the composite interface passivation layer in step S3 is as follows: First, oF-PEAI was dissolved in isopropanol, and then 2,3,6,7,10,11-hexahydroxytriphenylenebenzene and chlorobenzene were added to prepare a surface passivation solution; Then, the surface passivation solution is dripped onto the surface of the perovskite absorption layer, and the coating is performed by rotation at a rotation speed of 1500 to 2500 rpm for 20 to 50 seconds to passivate the top surface and obtain a composite interface passivation layer.

8. The method for preparing a thermally stable perovskite solar cell based on a composite interface passivation layer constructed by self-assembled discotic liquid crystal according to claim 1, It is characterized in that The method for forming the hole transport layer in step S4 is as follows: First, Spiro-OMeTAD, Li-TFSI acetonitrile solution and 4-tert-butylpyridine were mixed and dissolved in chlorobenzene, stirred at room temperature for 10 to 12 hours, and filtered through a 0.40 to 0.50 μm filter to prepare a Spiro-OMeTAD solution; The Spiro-OMeTAD solution is dropped onto the composite interface passivation layer for spin coating at a rotation speed of 4000-5000 rpm for 20-30 seconds to obtain a hole transport layer.

9. The method for preparing a thermally stable perovskite solar cell based on a composite interface passivation layer constructed by self-assembled discotic liquid crystal according to claim 1, It is characterized in that The electrode is a gold electrode with a thickness of 70-100 nm and an active area of ​​0.08-0.10 cm 2 .

10. A perovskite solar cell, It is characterized in that The method is prepared by any one of claims 1 to 9.

Citation Information

Cited By

  • Perovskite battery and preparation method thereof

    CN120035298A

  • Perovskite solar cell with modified hole transport layer and preparation method of perovskite solar cell

    CN120112059A

  • Method for optimizing interface layer and enhancing stability of perovskite solar cell

    CN120805737A