Tempered glass plate, method for producing tempered glass plate, and glass plate for strengthening
By adjusting the chemical composition of the glass and performing multiple ion exchange treatments, a reinforced glass plate with a compressive stress layer is formed, which solves the problem that the compression stress value and stress depth of the compression stress layer in the prior art is difficult to take into account, and it is not easy to break when falling effect.
Patent Information
- Application Number
- CN202380028713.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-11-28
- Filing Date
- 2023-04-20
- Publication Date
- 2024-11-05
AI Technical Summary
While the existing reinforced glass plates increase the compression stress value and stress depth of the compression stress layer, it is difficult to take into account both the high surface compression stress and the deep compression stress depth, resulting in easy breakage when falling.
By adjusting the chemical composition of the glass, the proportion of components such as SiO2, Al2O3, B2O3, Li2O, Na2O, K2O, etc. were increased, and multiple ion exchange treatments were performed to form a reinforced glass plate with a compressive stress layer on the surface, thereby improving the ion exchange performance of the glass. and fracture toughness.
Reinforced glass plates that are not easily damaged during falls are achieved, which improves the mechanical strength and acid resistance of the glass, and reduces the probability of damage of the protective glass.
Smart Images

Figure BDA0005049981970000351 
Figure BDA0005049981970000361 
Figure BDA0005049981970000371
Abstract
Description
Technical Field
[0001] The present invention relates to a tempered glass plate and a method for producing the same, and in particular to a tempered glass plate suitable for use as a cover glass for a touch panel display of a mobile phone, a digital camera, a PDA (portable terminal), etc., a method for producing the tempered glass plate, and a tempered glass plate. Background Art
[0002] In applications such as mobile phones (especially smart phones), digital cameras, and PDAs (personal digital assistants), an ion-exchange-treated tempered glass plate is used as a cover glass for a touch panel display (see Patent Document 1).
[0003] In addition, if a smartphone is accidentally dropped onto the road, the protective glass may be broken and the smartphone may not be usable. Therefore, in order to avoid such a situation, it is important to increase the strength of the tempered glass plate.
[0004] As a method of improving the strength of the tempered glass plate, deepening the stress depth is useful. Specifically, if the protective glass collides with the road surface when the smartphone falls, the protrusions and sand particles on the road surface will penetrate the protective glass and reach the tensile stress layer, causing damage. Therefore, if the stress depth of the compressive stress layer is deepened, it is difficult for protrusions and sand particles on the road surface to reach the tensile stress layer, which can reduce the probability of damage to the protective glass (see Patent Document 2).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2006-83045
[0008] Patent Document 2: Japanese Patent Application No. 2017-527513 Summary of the invention
[0009] Problems to be solved by the invention
[0010] According to the research of the inventors, in order to further improve the strength of the tempered glass plate, it is believed that it is useful to increase the compressive stress value at a depth corresponding to the size of the intrusion such as sand particles that causes the breakage (for example, a depth of 30 μm from the outermost surface). If it is a structure as described above, it is easy to suppress the damage from the inside of the tempered glass plate caused by the intrusion. However, in the previous glass (glass composition), even if the ion exchange conditions are changed to increase the compressive stress value at the specified depth, it is difficult to increase the compressive stress value at the specified depth. In addition, when the compressive stress value at the specified depth is increased, it is difficult to take into account both high surface compressive stress and deep compressive stress depth.
[0011] The present invention has been made in view of the above circumstances, and a technical object of the present invention is to provide a tempered glass plate which is less likely to be broken than conventional alkali-aluminosilicate glass and a method for producing the same.
[0012] Means for solving problems
[0013] (Invention 1) The tempered glass plate of the present invention is characterized in that it has a compressive stress layer on the surface, and contains, in mol%, SiO2 50-80%, Al2O3 7-25%, B2O3 0-15%, Li2O 0-15%, Na2O 0-25%, K2O 0-10%, MgO 0-15%, CaO 0-10%, SrO 0-10%, BaO 0-10%, ZnO 0-10%, P2O5 0-15%, TiO2 0-10%, ZrO2 0-10%, SnO2 0-0.30%, [B2O3]+[MgO]+[CaO] is 0.1-30%, and ([Li2O]+[Na2O]+[K2O]) / [Al2O3] is 0.5-2.0. Here, [B2O3] refers to the mole % content of B2O3. [MgO] refers to the mole % content of MgO. [CaO] refers to the mole % content of CaO. [Li2O] refers to the mole % content of Li2O. [Na2O] refers to the mole % content of Na2O. [K2O] refers to the mole % content of K2O. [Al2O3] refers to the mole % content of Al2O3. [B2O3]+[MgO]+[CaO] refers to the total content of B2O3, MgO and CaO. ([Li2O]+[Na2O]+[K2O]) / [Al2O3] refers to the value obtained by dividing the total content of Li2O, Na2O and K2O by the content of Al2O3.
[0014] (Invention 1-2) In addition, in the tempered glass plate of the present invention, it is preferred that the Z value calculated by the following formula is 18.0 or more.
[0015] Z=0.13×[SiO2]+2.36×[Al2O3]-0.14×[B2O3]+4.90×[Li2O]-5.53×[Na2O]-2.14×[MgO]-2.34×[CaO]
[0016] Here, [SiO2] refers to the mol% content of SiO2.
[0017] With such a configuration, it is possible to achieve both the efficiency of ion exchange between Li ions contained in the glass and Na ions in the molten salt and the efficiency of ion exchange between Na ions contained in the glass and K ions in the molten salt.
[0018] (Invention 1-3) In addition, in the tempered glass plate of the present invention, it is preferred that the Z value calculated by the following formula is 20.0 or more.
[0019] Z=0.13×[SiO2]+2.36×[Al2O3]-0.14×[B2O3]+4.90×[Li2O]-5.53×[Na2O]-2.14×[MgO]-2.34×[CaO]
[0020] (Invention 1-4) In addition, in the tempered glass plate of the present invention, it is preferred that the molar ratio [Na2O] / [Li2O] is 1.0 or less.
[0021] With such a configuration, the efficiency of ion exchange between Li ions contained in the glass and Na ions in the molten salt can be improved.
[0022] (Invention 1-5) In addition, in the tempered glass plate of the present invention, it is preferred that the Y value calculated by the following formula is 5.0 or more.
[0023] Y=3+0.21×[SiO2]+0.25×[Al2O3]-0.33×[B2O3]-0.55×[Li2O]+0.45×[Na2O]-0.97×[MgO]-1.46×[CaO]
[0024] Here, [SiO2] refers to the mol% content of SiO2.
[0025] With such a configuration, the efficiency of ion exchange between Na ions contained in the glass and K ions in the molten salt can be improved.
[0026] (Invention 1-6) In addition, for the tempered glass plate of the present invention, it is preferred that the Y value calculated by the following formula is 6.0 to 30.
[0027] Y=3+0.21×[SiO2]+0.25×[Al2O3]-0.33×[B2O3]-0.55×[Li2O]+0.45×[Na2O]-0.97×[MgO]-1.46×[CaO]
[0028] With such a configuration, the efficiency of the ion exchange between the Na ions contained in the glass and the K ions in the molten salt can be further improved.
[0029] (Invention 1-7) In addition, in the tempered glass plate of the present invention, it is preferred that the X value calculated by the following formula is 300 or more.
[0030] X=-1.49×[SiO2]+26.98×[Al2O3]-3.23×[B2O3]+48.56×[Li2O]-24.31×[Na2O]-0.28×[MgO]+2.74×[CaO]
[0031] With such a configuration, the efficiency of ion exchange between Li ions contained in the glass and Na ions in the molten salt can be improved.
[0032] (Invention 1-8) In addition, for the tempered glass plate of the present invention, it is preferred that the W value calculated by the following formula is 340 or more.
[0033] W=0.07×[SiO2]+18.17×[Al2O3]-4.42×[B2O3]+41.43×[Li2O]-29.30×[Na2O]+1.43×[MgO]-10.43×[CaO]
[0034] With such a configuration, the Young's modulus of the tempered glass sheet can be increased.
[0035] (Invention 1-9) In addition, in the tempered glass plate of the present invention, it is preferred that [Al2O3]+[Li2O]+[Na2O]+[K2O] is 10.5% or more.
[0036] With such a configuration, the ion exchange performance of the tempered glass sheet can be improved.
[0037] (Invention 1-10) In addition, in the tempered glass plate of the present invention, it is preferred that the molar ratio [Li2O] / [Al2O3] is 0.1 or more.
[0038] With such a configuration, the ion exchange performance of the tempered glass sheet can be further improved.
[0039] (Invention 1-11) In addition, for the tempered glass plate of the present invention, it is preferred that the U value calculated by the following formula is 7000 or more.
[0040] U=87.39×[SiO2]+180.12×[Al2O3]+93.63×[B2O3]+113.78×
[0041] ([MgO]+[CaO]+[BaO]+[SrO])-46.2×[Li2O]-71.1×[Na2O]-58.6×[K2O]-40.0×[P2O5]
[0042] With such a configuration, the fracture toughness K1c of the tempered glass plate can be improved.
[0043] (Invention 1-12) In addition, for the tempered glass plate of the present invention, it is preferred that Q = [SiO2] + 1.2×[P2O5] - 3×[Al2O3] - [B2O3] - 2×[Li2O] - 1.5×[Na2O] - [K2O] is greater than -30%.
[0044] With such a configuration, the acid resistance of the tempered glass plate can be improved.
[0045] (Invention 1-13) In addition, the tempered glass plate of the present invention preferably contains Cl as a glass composition, and the content of Cl is preferably 0.02 mol% or more.
[0046] With such a configuration, the diameter of bubbles in the molten glass can be easily enlarged, and a high clarification effect can be obtained.
[0047] (Invention 1-14) In addition, for the tempered glass plate of the present invention, it is preferred that the glass composition contains MoO 3, and the content of MoO 3 is 0.0001 mol% or more.
[0048] With such a configuration, the tempered glass plate easily absorbs ultraviolet rays, and degradation of elements inside the device due to ultraviolet rays can be suppressed.
[0049] (Invention 1-15) In addition, the tempered glass plate of the present invention preferably has a softening point (Ts) of 920° C. or less. Here, the “softening point” refers to a value measured by a method based on ASTM C338.
[0050] With such a configuration, it is easy to reduce the manufacturing cost of the tempered glass sheet when the tempered glass sheet is bent.
[0051] (Invention 1-16) In addition, for the tempered glass plate of the present invention, it is preferred that the compressive stress value CS of the outermost surface of the compressive stress layer is 200 to 1200 MPa, and the stress depth DOC of the compressive stress layer is 3 to 200 μm. Here, for the "compressive stress value of the outermost surface" and "stress depth", for example, when the compressive stress is caused by potassium ions introduced by ion exchange, it refers to the value measured using FSM-6000 (manufactured by Orihara Seisakusho Co., Ltd.), and when the compressive stress is caused by Na ions introduced by ion exchange, it refers to the value measured based on the phase difference distribution curve observed using the scattered light photoelastic stress meter SLP-2000 (manufactured by Orihara Seisakusho Co., Ltd.). And, the stress depth refers to the depth at which the stress value becomes zero. It should be noted that in the calculation of the stress characteristics of each sample, the refractive index and the photoelastic constant are used. The refractive index uses the value measured by the V-block method. The photoelastic constant uses the value measured by the optical heterodyne measurement method.
[0052] With such a configuration, a strengthened glass sheet with high strength can be obtained.
[0053] (Invention 1-17) Additionally, for the strengthened glass sheet of the present invention, preferably, the stress depth DOC of the compressive stress layer is 50 to 200 μm, and the compressive stress value CS30 at a depth of 30 μm from the outermost surface is 35 to 400 MPa.
[0054] With such a configuration, a strengthened glass sheet that is not easily broken when dropped can be obtained.
[0055] (Invention 1-18) Additionally, for the strengthened glass sheet of the present invention, preferably, the compressive stress CS30 at a depth of 30 μm from the surface is 120 MPa or more and the compressive stress CS at the outermost surface is 400 MPa or more.
[0056] With such a configuration, higher internal stress can be obtained, and the drop strength of the protective glass for smartphones can be improved.
[0057] (Invention 1-19) Additionally, for the strengthened glass sheet of the present invention, preferably, the temperature at a high-temperature viscosity of 10 2.5 dPa·s is 1680 °C or lower. Here, the "temperature at a high-temperature viscosity of 10 2.5 dPa·s" can be measured, for example, by the platinum ball pulling method.
[0058] With such a configuration, the molten glass is easily formed into a plate shape.
[0059] (Invention 1-20) Additionally, for the strengthened glass sheet of the present invention, preferably, an overflow confluence surface (Japanese original text: オ一バ一フロ一合流面) is provided at the central portion in the plate thickness direction. Here, the "overflow down-draw method" is a method of manufacturing a glass sheet by causing molten glass to overflow from both sides of a forming body refractory, causing the overflowed molten glass to converge at the lower end of the forming body refractory, and stretching it downward while forming.
[0060] With such a configuration, an unpolished strengthened glass sheet with good surface quality can be manufactured at low cost.
[0061] (Invention 1-21) Additionally, for the strengthened glass sheet of the present invention, preferably, the stress curve in the thickness direction is bent.
[0062] With such a configuration, a strengthened glass sheet with a high compressive stress on the surface and a deep stress depth can be obtained.
[0063] (Invention 1-22) Additionally, for the strengthened glass sheet of the present invention, preferably, the mutual diffusion coefficient D of Na ions (substantially Na ions and Li ions) in the deep region at 380 °CNa 1×10 -14 ~1×10 -11 m 2 sec -1 The mutual diffusion coefficient D of K ions (essentially K ions and Na ions) in the shallow area at this temperature is K 1×10 -17 ~1×10 - 14 m 2 sec -1 , and their ratio D K / D Na It is 0.0001 or more.
[0064] (Invention 1-23) In addition, for the tempered glass plate of the present invention, it is preferred that the Na ion mutual diffusion coefficient D when ion exchange is carried out in NaNO3 at 380°C is Na 1×10 -14 ~1×10 -11 m 2 sec -1 , the K ion mutual diffusion coefficient D when ion exchange was carried out in KNO3 at 380℃ K 1×10 -17 ~1×10 -14 m 2 sec -1 , and their ratio D K / D Na It is 0.0001 or more.
[0065] (Invention 2) The tempered glass plate of the present invention is characterized in that, as a glass composition, it contains, in mol%, SiO2 50-80%, Al2O3 7-25%, B2O3 1-15%, Li2O 0-15%, Na2O 0-25%, K2O 0-10%, MgO 0-15%, CaO 0-10%, BaO 0-10%, SrO 0-10%, ZnO 0-10%, P2O5 0-4%, TiO2 0.001-0.1%, ZrO2 0-10%, Fe2O3 0.001-0.1%, SnO2 0.001~0.30%, [B2O3]+[MgO]+[CaO] is 0.1~30%, and ([Li2O]+[Na2O]+[K2O]) / [Al2O3] is 0.5~2.0.
[0066] (Invention 3) In addition, the method for producing a tempered glass plate of the present invention is characterized by comprising the following steps: a preparation step of preparing the tempered glass plate, wherein the tempered glass plate contains, as a glass composition, SiO2 50-80%, Al2O3 7-25%, B2O3 0-15%, Li2O 0-15%, Na2O 0-25%, K2O 0-10%, MgO 0-15%, CaO 0-10%, BaO 0-10%, SrO 0-10%, ZnO 0-10%, P2O5 0-15%, TiO2 0-10%, ZrO2 0-10%, SnO2 0~0.30%, [B2O3]+[MgO]+[CaO] is 0.1~30%, and ([Li2O]+[Na2O]+[K2O]) / [Al2O3] is 0.5~2.0; and an ion exchange process, wherein the strengthened glass plate is subjected to multiple ion exchange treatments to obtain a strengthened glass plate having a compressive stress layer on the surface.
[0067] (Invention 4) In addition, the tempered glass plate of the present invention is characterized in that, as a glass composition, it contains, in mol%, SiO2 50 to 80%, Al2O3 7 to 25%, B2O3 0 to 15%, Li2O 0 to 15%, Na2O 0 to 25%, K2O 0 to 10%, MgO 0 to 15%, CaO 0 to 10%, BaO 0 to 10%, SrO 0 to 10%, ZnO 0 to 10%, P2O5 0 to 15%, TiO2 0 to 10%, ZrO2 0 to 10%, SnO2 0 to 0.30%, [B2O3] + [MgO] + [CaO] is 0.1 to 30%, and ([Li2O] + [Na2O] + [K2O]) / [Al2O3] is 0.5 to 2.0.
[0068] (Invention 4-1) In addition, for the tempered glass plate of the present invention, it is preferred that the Na ion mutual diffusion coefficient D when ion exchange is carried out in NaNO3 at 380°C is Na 1×10 -14 ~1×10 -11 m 2 sec -1 , the K ion mutual diffusion coefficient D when ion exchange was carried out in KNO3 at 380℃ K 1×10 -17 ~1×10 -14 m 2 sec -1 , and their ratio D K / D Na It is 0.001 or more.
[0069] With such a configuration, when the compressive stress value at a predetermined depth (for example, a depth of 30 μm from the outermost surface) is increased, it is possible to achieve both high surface compressive stress and deep compressive stress depth.
[0070] (Invention 4-2) In addition, in the tempered glass plate of the present invention, it is preferred that the Z value calculated by the following formula is 18.0 or more.
[0071] Z=0.13×[SiO2]+2.36×[Al2O3]-0.14×[B2O3]+4.90×[Li2O]-5.53×[Na2O]-2.14×[MgO]-2.34×[CaO]
[0072] (Invention 4-3) In addition, in the tempered glass plate of the present invention, it is preferred that the Z value calculated by the following formula is 20.0 or more.
[0073] Z=0.13×[SiO2]+2.36×[Al2O3]-0.14×[B2O3]+4.90×[Li2O]-5.53×[Na2O]-2.14×[MgO]-2.34×[CaO]
[0074] (Invention 4-4) In addition, in the tempered glass plate of the present invention, it is preferred that the molar ratio [Na2O] / [Li2O] is 1.0 or less.
[0075] (Invention 4-5) In addition, in the tempered glass plate of the present invention, it is preferred that the Y value calculated by the following formula is 5.0 or more.
[0076] Y=3+0.21×[SiO2]+0.25×[Al2O3]-0.33×[B2O3]-0.55×[Li2O]+0.45×[Na2O]-0.97×[MgO]-1.46×[CaO]
[0077] (Invention 4-6) In addition, for the tempered glass plate of the present invention, it is preferred that the Y value calculated by the following formula is 6.0 to 30.
[0078] Y=3+0.21×[SiO2]+0.25×[Al2O3]-0.33×[B2O3]-0.55×[Li2O]+0.45×[Na2O]-0.97×[MgO]-1.46×[CaO]
[0079] (Invention 4-7) In addition, in the tempered glass plate of the present invention, it is preferred that the X value calculated by the following formula is 300 or more.
[0080] X=-1.49×[SiO2]+26.98×[Al2O3]-3.23×[B2O3]+48.56×[Li2O]-24.31×[Na2O]-0.28×[MgO]+2.74×[CaO]
[0081] (Invention 4-8) In addition, for the tempered glass plate of the present invention, it is preferred that the W value calculated by the following formula is 340 or more.
[0082] W=0.07×[SiO2]+18.17×[Al2O3]-4.42×[B2O3]+41.43×[Li2O]-29.30×[Na2O]+1.43×[MgO]-10.43×[CaO]
[0083] (Invention 4-9) In addition, in the tempered glass plate of the present invention, it is preferred that [Al2O3]+[Li2O]+[Na2O]+[K2O] is 10.5% or more.
[0084] (Invention 4-10) In addition, in the tempered glass plate of the present invention, it is preferred that the molar ratio [Li2O] / [Al2O3] is 0.1 or more.
[0085] (Invention 4-11) In addition, for the tempered glass plate of the present invention, it is preferred that the U value calculated by the following formula is 7000 or more.
[0086] U=87.39×[SiO2]+180.12×[Al2O3]+93.63×[B2O3]+113.78×([MgO]+[CaO]+[BaO]+[SrO])-46.2×[Li2O]-71.1×[Na2O]-58.6×[K2O]-40.0×[P2O5]
[0087] (Invention 4-12) In addition, for the tempered glass plate of the present invention, it is preferred that Q = [SiO2] + 1.2×[P2O5] - 3×[Al2O3] - [B2O3] - 2×[Li2O] - 1.5×[Na2O] - [K2O] is greater than -30%.
[0088] (Invention 4-13) In addition, the tempered glass plate of the present invention preferably contains C1 as a glass composition, and the content of C1 is preferably 0.02 mol% or more.
[0089] (Invention 4-14) In addition, for the tempered glass plate of the present invention, it is preferred that the glass composition contains MoO 3, and the content of MoO 3 is 0.0001 mol% or more.
[0090] (Invention 4-15) In addition, the tempered glass plate of the present invention preferably has a softening point (Ts) of 920° C. or less. Here, the “softening point” refers to a value measured by a method based on ASTM C338.
[0091] (Invention 5) In addition, the method for manufacturing a tempered glass plate of the present invention is characterized by comprising the following steps: a preparation step of preparing a tempered glass plate in which the Na ion mutual diffusion coefficient D when ion exchange is performed in NaNO3 at 380°C is Na 1×10 -14 ~1×10 -11 m 2 sec -1 , the K ion mutual diffusion coefficient D when ion exchange was carried out in KNO3 at 380℃ K 1×10 -17 ~1×10 -14 m 2 sec -1 , and their ratio D K / D Na is 0.001 or more; and an ion exchange step of subjecting the strengthened glass plate to a plurality of ion exchange treatments to obtain a strengthened glass plate having a compressive stress layer on the surface.
[0092] Effects of the Invention
[0093] According to the present invention, it is possible to provide a tempered glass plate which is less likely to be broken when dropped than conventional alkali-aluminosilicate glass, and a method for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0094] Figure 1 It is an explanatory diagram illustrating a stress curve having a first peak a, a first valley b, a second peak c, and a second valley d.
[0095] Figure 2 Yes Figure 1 An enlarged illustration of the low compressive stress region in the stress curve shown.
[0096] Figure 3 It is an explanatory diagram illustrating a stress curve having an inflection point (original Japanese: buckling point) e.
[0097] Figure 4 It is a graph showing stress curves of Examples 2-1 to 2-3.
[0098] Figure 5 Yes Figure 4 The diagram shows an enlarged view of the low compressive stress region in the stress curves of Examples 2-1 to 2-3.
[0099] Figure 6It is a graph showing stress curves of Examples 3-1 and 3-2.
[0100] Figure 7 Yes Figure 6 The diagram shows an enlarged view of the low compressive stress region in the stress curves of Examples 3-1 and 3-2.
[0101] Figure 8 It is a graph showing stress curves of Examples 4-1 to 4-4.
[0102] Fig. 9 Yes Figure 8 The diagram shows an enlarged view of the low compressive stress region in the stress curves of Examples 4-1 to 4-4.
[0103] Fig.10 This is an explanatory diagram illustrating a Na ion concentration curve measured by EPMA. DETAILED DESCRIPTION
[0104] The tempered glass plate in the present invention refers to a glass plate that has been subjected to ion exchange treatment and has a compressive stress layer on the surface. The tempered glass plate refers to a glass plate that has not been subjected to the above ion exchange (before ion exchange).
[0105] The tempered glass plate (tempered glass plate) of the present invention contains, as a glass composition, SiO2 50-80%, Al2O3 7-25%, B2O3 0-15%, Li2O 0-15%, Na2O 0-25%, K2O 0-10%, MgO 0-15%, CaO 0-10%, BaO 0-10%, SrO 0-10%, ZnO 0-10%, P2O5 0-15%, TiO2 0-10%, ZrO2 0-10%, SnO2 0-0.30%, [B2O3] + [MgO] + [CaO] is 0.1-30%, and ([Li2O] + [Na2O] + [K2O]) / [Al2O3] is 0.5-2.0. The reasons for limiting the content range of each component are shown below. In addition, in the description of the content range of each component, unless otherwise specified, % means mole %.
[0106] SiO2 is a component that forms a glass network. If the content of SiO2 is too little, it is difficult to vitrify. In addition, the thermal expansion coefficient becomes too high, and the thermal shock resistance is easily reduced. Therefore, the suitable lower limit range of SiO2 is more than 50%, more than 52%, more than 55%, more than 57%, more than 58%, more than 58.5%, more than 59%, more than 60%, more than 61%, more than 62%, more than 62.5%, more than 63%, and especially more than 63.5%. On the other hand, if the content of SiO2 is too much, the solubility and formability are easily reduced. In addition, the thermal expansion coefficient becomes too low, and it is difficult to match the thermal expansion coefficient of the surrounding materials. Therefore, the suitable upper limit range of SiO2 is less than 80%, less than 75%, less than 73%, less than 72%, less than 71%, less than 70.5%, less than 70%, less than 69.5%, less than 69%, less than 68.5%, less than 68%, less than 67.8%, less than 67.5%, less than 67.2%, and especially less than 67%.
[0107] Al2O3 is a component that improves ion exchange performance, and is a component that improves strain point, Young's modulus, fracture toughness, and Vickers hardness. Therefore, the suitable lower limit range of Al2O3 is more than 7%, more than 7.2%, more than 7.5%, more than 7.8%, more than 8%, more than 8.2%, more than 8.5%, more than 9%, more than 9.2%, more than 9.4%, more than 9.5%, more than 9.8%, more than 10.0%, more than 10.3%, more than 10.5%, more than 10.8%, more than 11%, more than 11.2%, more than 11.4%, more than 11.6%, especially more than 11.8%. On the other hand, if the content of Al2O3 is too much, the high temperature viscosity rises, and the melting property and formability are easily reduced. In addition, devitrified crystals are easily precipitated in the glass, and it is difficult to form it into a plate shape using overflow down-drawing method, etc. Particularly, when using alumina-based refractory as a formed body refractory, utilizing overflow downdrawing method to be formed into a plate-like state, devitrified crystals of spinel are easily precipitated at the interface with alumina-based refractory. In addition, acid resistance is reduced, and it is difficult to be applied to acid treatment process. Therefore, Al2O3's suitable upper limit range is below 25%, below 23%, below 21%, below 20.5%, below 20%, below 19.8%, below 19.5%, below 19.0%, below 18.5%, below 18%, below 17.5%, below 17%, below 16.5%, below 15.5%, below 15.2%, below 15%, below 14.9%, below 14.7%, below 14.5%, below 14.3%, below 14%, below 13.5, and particularly below 13%. If the content of Al 2 O 3 , which has a great influence on the ion exchange performance, is set in an appropriate range, it is easy to form a curve having a first peak a, a first valley b, a second peak c, and a second valley d.
[0108] B2O3 is a component that reduces high temperature viscosity and density, stabilizes the glass, makes crystals difficult to precipitate, and reduces the liquidus temperature. It is also a component that increases fracture toughness K1c and fracture energy γ. It is also a component that increases the binding force of cations on oxygen electrons and reduces the basicity of the glass. If the content of B2O3 is too low, the stress depth (DOC) in the ion exchange between Li ions contained in the glass and Na ions in the molten salt will increase. Na ) becomes too deep, and as a result, the compressive stress value at a predetermined depth (5 to 50 μm) from the outermost surface tends to become smaller. In addition, the glass becomes unstable and the resistance to devitrification may also be reduced. In addition, the alkalinity of the glass becomes too large, the amount of O2 released by the reaction of the clarifier decreases, the foaming property decreases, and bubbles may remain in the glass during plate forming. Therefore, the suitable lower limit range of B2O3 is 0% or more, 0.10% or more, 0.15% or more, 0.20% or more, 0.30% or more, 0.4% or more, 0.5% or more, 0.6% or more, 0.7% or more, 0.8% or more, 0.9% or more, 1% or more, 1.5% or more, 2% or more, 2.5% or more, 3% or more, 3.5% or more, 4% or more, and especially 4.5% or more. On the other hand, if the content of B2O3 is too much, the stress depth may become shallow. In particular, the efficiency of ion exchange between Na ions contained in the glass and K ions in the molten salt is easily reduced, and the diffusion of K ions is easily reduced. Therefore, the upper limit range of B2O3 is 15% or less, 14.5% or less, 14% or less, 13.5% or less, 13% or less, 12.5% or less, 12% or less, 11.5% or less, 11% or less, 10.5% or less, 10% or less, 9.5% or less, 9% or less, 8.5% or less, 8% or less, 7.5% or less, 7% or less, 6.5% or less, 6% or less, and particularly 5.5% or less. If the content of B2O3 is set to a suitable range, it is easy to form a curve having the first peak a, the first valley b, the second peak c, and the second valley d.
[0109] Li2O is an ion exchange component, and is particularly a component necessary for obtaining a deep stress depth by ion exchange between Li ions contained in the glass and Na ions in the molten salt. In addition, Li2O is a component that reduces high temperature viscosity, improves solubility and formability, and is a component that improves Young's modulus. Therefore, the suitable lower limit range of Li2O is 0% or more, 0.1% or more, 0.5% or more, 1% or more, 1.5% or more, 2% or more, 2.5% or more, 3% or more, 3.5% or more, 4% or more, 4.3% or more, 4.5% or more, 4.7% or more, 5% or more, 5.2% or more, 5.5% or more, 5.8% or more, and particularly 6.0% or more. In addition, the suitable upper limit range of Li2O is less than 15%, less than 13%, less than 12%, less than 11.5%, less than 11%, less than 10.5%, less than 10%, less than 9.8%, less than 9.5%, less than 9.3%, less than 9%, less than 8.8%, less than 8.5%, less than 8.2%, and especially less than 8.0%.
[0110] Na2O is an ion exchange component, and is a component that reduces high temperature viscosity, improves solubility and formability. In addition, Na2O is a component that improves devitrification resistance, and is particularly a component that suppresses devitrification produced in the reaction with alumina-based refractory materials. Therefore, the suitable lower limit range of Na2O is 0% or more, 0.5% or more, 1% or more, 1.2% or more, 1.5% or more, 1.8% or more, 2% or more, 2.1% or more, 2.3% or more, 2.5%, 2.8% or more, 3% or more, 3.2% or more, 3.5% or more, 4% or more, 4.5% or more, 5% or more, 5.5% or more, 6% or more, 6.5 or more, and particularly 7% or more. On the other hand, if the content of Na2O is too much, the thermal expansion coefficient becomes too high, and the thermal shock resistance is easily reduced. In addition, sometimes the components of the glass composition are unbalanced, and the devitrification resistance is reduced instead. Therefore, the suitable upper limit range of Na2O is 25% or less, 21% or less, 20% or less, 19% or less, especially 18% or less, 15% or less, 13% or less, 11% or less, especially 10% or less.
[0111] K2O is a component that reduces high temperature viscosity and improves solubility and formability. In addition, it is a component that deepens the stress depth. Therefore, the suitable lower limit range of K2O is more than 0%, more than 0.01%, more than 0.02%, more than 0.03%, more than 0.05%, more than 0.08%, more than 0.1%, more than 0.2%, more than 0.3%, more than 0.4%, and especially more than 0.5%. On the other hand, if the content of K2O is too much, the thermal expansion coefficient becomes higher and the heat shock resistance may decrease. In addition, the compressive stress value of the outermost surface is easy to decrease. Therefore, the suitable upper limit range of K2O is less than 10%, less than 7%, less than 6%, less than 5%, less than 4%, less than 3%, less than 2%, less than 1.5%, less than 1%, and especially less than 1%.
[0112] MgO is a component that reduces high temperature viscosity, improves solubility and formability, and improves strain point and Vickers hardness. It is a component that has a large effect of improving ion exchange performance among alkaline earth metal oxides. Therefore, the suitable lower limit range of MgO is more than 0%, more than 0.03%, more than 0.05%, more than 0.07%, more than 0.10%, more than 0.15%, more than 0.2%, more than 0.5%, more than 0.6%, more than 0.7%, more than 1.0%, more than 1.5%, and especially more than 1.8%. On the other hand, if the content of MgO is too much, the devitrification resistance is easily reduced, and it is particularly difficult to suppress the devitrification produced in the reaction with alumina-based refractory. Therefore, the suitable upper limit range of MgO is less than 15%, less than 12%, less than 11%, less than 10%, less than 8%, less than 7%, less than 6.5%, less than 6%, less than 5.5%, less than 5%, less than 4.7%, less than 4.5%, less than 4.2%, less than 4%, less than 3.8%, and especially less than 3.5%.
[0113] Compared with other components, CaO is a component that reduces high temperature viscosity without decreasing devitrification resistance, improves solubility and formability, and increases strain point and Vickers hardness. However, if the content of CaO is too much, it is possible that the ion exchange performance is reduced and the ion exchange solution is deteriorated during ion exchange treatment. Therefore, the content of CaO is preferably 0-10%, 0-9%, 0-8%, 0-7%, 0-6%, 0-5.5%, 0-5%, 0-4.5%, 0-4%, 0-3.5%, 0-3%, 0-2%, 0-1%, 0-less than 1%, 0-0.7%, 0-0.5%, 0-0.3%, 0-0.1%, 0-0.05%, 0-0.02%, and particularly preferably 0-less than 0.01%. It should be noted that when CaO is allowed to be mixed as an impurity, it is preferably 0.01% or more, 0.02% or more, and particularly preferably 0.03% or more.
[0114] SrO is a component that reduces high temperature viscosity, improves solubility and formability, or increases strain point and Young's modulus. However, if its content is too high, the ion exchange reaction is easily inhibited, and the density and thermal expansion coefficient become unduly high, or the glass is easily devitrified. Therefore, the SrO content is preferably 0 to 2%, 0 to 1.5%, 0 to 1%, 0 to 0.5%, 0 to 0.1%, and particularly preferably 0 to less than 0.1%.
[0115] BaO is a component that reduces high temperature viscosity, improves solubility and formability, or increases strain point and Young's modulus. However, if its content is too high, the ion exchange reaction is easily inhibited, and the density and thermal expansion coefficient become unduly high, and the glass is easily devitrified. Therefore, the content of BaO is preferably 0 to 2%, 0 to 1.5%, 0 to 1%, 0 to 0.5%, 0 to 0.1%, and particularly preferably 0 to less than 0.1%.
[0116] ZnO is a component that improves ion exchange performance, and is particularly effective in increasing the compressive stress value of the outermost surface of the compressive stress layer. In addition, it is a component that reduces high-temperature viscosity without significantly reducing low-temperature viscosity. On the other hand, if the ZnO content is too much, there is a tendency for glass phase separation, or reduced devitrification resistance, or increased density, or shallower stress depth. Therefore, the suitable upper limit range of ZnO is 10% or less, 8% or less, 7% or less, 6% or less, 5.5% or less, 5.2% or less, 5% or less, 4.5% or less, and particularly 4% or less. The suitable lower limit range of ZnO is 0% or more, 0.1% or more, 0.2% or more, 0.3% or more, 0.4% or more, 0.5% or more, 0.7% or more, 1% or more, 1.1% or more, 1.2% or more, 1.5% or more, 1.8% or more, 2.0% or more, 2.1% or more, 2.2% or more, 2.5% or more, 2.8% or more, 3.0% or more, 3.1% or more, 3.2% or more, and especially 3.5% or more.
[0117] P2O5 is a component that improves ion exchange performance, especially a component that deepens the stress depth. In addition, it is a component that also improves acid resistance. In addition, it is a component that increases the binding force of cations on oxygen electrons and reduces the basicity of glass. However, if the content of P2O5 is too much, the glass will easily separate and the water resistance will be reduced. In addition, the stress depth (DOC) in the ion exchange between Li ions contained in the glass and Na ions in the molten salt is Na) becomes too deep, and as a result, the compressive stress value at a predetermined depth (5 to 50 μm) from the outermost surface tends to become smaller. Therefore, the suitable upper limit range of P2O5 is less than 15%, less than 10%, less than 8%, less than 7%, less than 6%, less than 5%, less than 4.7%, less than 4.5%, less than 4%, and especially less than 3.5%. If the content of P2O5 is set to a suitable range, a non-monotonic curve is likely to be formed. On the other hand, if the content of P2O5 is too little, the ion exchange performance may not be fully exerted. In particular, the efficiency of ion exchange between Na ions contained in the glass and K ions in the molten salt is likely to decrease, and the diffusion of K ions is likely to decrease. In addition, the glass becomes unstable and the resistance to devitrification may also decrease. In addition, the alkalinity of the glass becomes too large, the amount of O2 released by the reaction of the clarifier decreases, the foaming property decreases, and bubbles may remain in the glass during plate forming. Therefore, the suitable lower limit range of P2O5 is above 0%, above 0.01%, above 0.02%, above 0.03%, above 0.05%, above 0.1%, above 0.4%, above 0.7%, above 1%, above 1.2%, above 1.4%, above 1.6%, above 2%, above 2.3%, and especially above 2.5%.
[0118] SnO2 is a clarifier and a component that improves ion exchange performance, but if its content is too high, the resistance to devitrification tends to decrease. Therefore, the suitable lower limit range of SnO2 is above 0%, above 0.001%, above 0.002%, above 0.005%, above 0.007%, and especially above 0.010%, and the suitable upper limit range is below 0.30%, below 0.27%, below 0.25%, below 0.20%, below 0.18%, below 0.15%, below 0.12%, below 0.10%, below 0.09%, below 0.08%, below 0.07%, below 0.06%, below 0.05%, below 0.047%, below 0.045%, below 0.042%, below 0.040%, below 0.038%, below 0.035%, below 0.032%, below 0.030%, below 0.025%, below 0.020%, and especially below 0.015%.
[0119] Cl is a clarifier. In particular, by using it in combination with SnO2, the bubble diameter in the glass is easily enlarged, and the clarification effect is easily exerted. On the other hand, if its content is too much, it is a component that has an adverse effect on the environment and equipment. Therefore, the suitable lower limit range of Cl is 0.001% or more, 0.005% or more, 0.008% or more, 0.010% or more, 0.015% or more, 0.018% or more, 0.019% or more, 0.020% or more, 0.023% or more, 0.025% or more, 0.027% or more, 0.030% or more, 0.035% or more, 0.040% or more, 0.050% or more, 0.07% or more, 0.09% or more, especially 0.10% or more, and the suitable upper limit range is 0.3% or less, 0.2% or less, 0.17% or less, 0.15% or less, especially 0.12% or less.
[0120] MoO3 is a component that absorbs ultraviolet rays (light with a wavelength of 200 to 300 nm). By containing MoO3 in the glass, it is possible to suppress the degradation of internal components of a device that uses the tempered glass plate of the present invention as protective glass due to ultraviolet rays. In addition, MoO3 is also a component mixed in from the manufacturing process. In particular, when the raw material batch is melted by electric melting heating, it is mixed in by dissolution from the Mo electrode. By using electric melting, the amount of water in the glass can be reduced. If the amount of water in the glass is reduced, the liquidus viscosity and the strain point increase, which can improve the resistance to devitrification and heat resistance of the glass. In addition, by increasing the strain point, it becomes difficult to produce stress relaxation, and a high compressive stress value can be maintained. If the content of MoO3 is too little, electric melting that may mix MoO3 cannot be used, and the above-mentioned effect cannot be obtained. Therefore, the suitable lower limit range of the content of MoO3 is 0% or more, 0.0001% or more, 0.0003% or more, 0.0005% or more, 0.0008% or more, 0.001% or more, 0.0012% or more, 0.0015% or more, and particularly 0.002% or more. On the other hand, if the content of MoO3 is too much, the transmittance of the protective glass is easily reduced. Therefore, the suitable upper limit range of the content of MoO3 is 0.02% or less, 0.018% or less, 0.015% or less, 0.012% or less, 0.01% or less, 0.008% or less, 0.007% or less, 0.006% or less, 0.005% or less, and particularly less than 0.004%.
[0121] The suitable lower limit range of the total content of B2O3, MgO and CaO, i.e., [B2O3] + [MgO] + [CaO], is 0.1% or more, 0.5% or more, 0.8% or more, 1% or more, 2% or more, 3% or more, 3.5% or more, 4% or more, 5% or more, 6% or more, 6.5% or more, and especially 7% or more. If [B2O3] + [MgO] + [CaO] is too little, it is difficult to lower the softening point. On the other hand, if [B2O3] + [MgO] + [CaO] is too much, the glass becomes unstable and the resistance to devitrification may be reduced. Therefore, the suitable upper limit range of [B2O3] + [MgO] + [CaO] is 30% or less, 28% or less, 25% or less, 24% or less, 22% or less, 20% or less, and especially 18% or less.
[0122] The suitable lower limit range of the total content of Li2O, Na2O and K2O, i.e., [Li2O] + [Na2O] + [K2O], is 7% or more, 7.5% or more, 8% or more, 8.5% or more, 8.8% or more, 9% or more, 9.5% or more, 9.7% or more, 10% or more, 10.2% or more, and especially 10.5% or more. If [Li2O] + [Na2O] + [K2O] is too little, the efficiency of ion exchange is likely to decrease, and it is difficult to achieve a low softening point. On the other hand, if [Li2O] + [Na2O] + [K2O] is too much, the chemical resistance may decrease. The suitable upper limit range of [Li2O] + [Na2O] + [K2O] is 30% or less, 28% or less, 25% or less, 24% or less, and especially 23% or less.
[0123] The suitable lower limit range of the total content of Al2O3, Li2O, Na2O and K2O, i.e., [Al2O3]+[Li2O]+[Na2O]+[K2O], is 10.5% or more, 11% or more, 11.5% or more, 12.0% or more, 12.3% or more, 12.5% or more, 13.0% or more, 14.0% or more, 15% or more, 16% or more, 18% or more, 19% or more, 20% or more, 21% or more, 24% or more, 25% or more, 28% or more, and especially 30% or more. If [Al2O3]+[Li2O]+[Na2O]+[K2O] is too little, the efficiency of ion exchange is easily reduced, and it is difficult to reduce the softening point. On the other hand, if [Al2O3]+[Li2O]+[Na2O]+[K2O] is too much, the liquid viscosity may be reduced and the chemical resistance may be reduced. The suitable upper limit range of [Al2O3]+[Li2O]+[Na2O]+[K2O] is 45% or less, 40% or less, 38% or less, 35% or less, and particularly 33% or less.
[0124] The suitable lower limit range of the molar ratio ([Li2O] + [Na2O] + [K2O]) / [Al2O3] is 0.5 or more, 0.6 or more, 0.7 or more, 0.75 or more, 0.8 or more, 0.85 or more, 0.9 or more, and particularly 0.95 or more. If the molar ratio ([Li2O] + [Na2O] + [K2O]) / [Al2O3] is too small, the efficiency of ion exchange is easily reduced. On the other hand, even if the molar ratio ([Li2O] + [Na2O] + [K2O]) / [Al2O3] is too large, the efficiency of ion exchange is also easily reduced. Therefore, the suitable upper limit range of the molar ratio ([Li2O] + [Na2O] + [K2O]) / [Al2O3] is 2.0 or less, 1.8 or less, 1.9 or less, 1.8 or less, 1.7 or less, 1.6 or less, 1.5 or less, 1.4 or less, and particularly 1.3 or less. It should be noted that “([Li2O]+[Na2O]+[K2O]) / [Al2O3]” refers to a value obtained by dividing the total content of Li2O, Na2O and K2O by the content of Al2O3.
[0125] The suitable upper limit range of the molar ratio [Al2O3] / ([R2O]+[RO]) is 1.5 or less, 1.4 or less, 1.3 or less, 1.2 or less, 1.1 or less, 1 or less, and particularly 0.9 or less. If [Al2O3] / ([R2O]+[RO]) is too large, the high temperature viscosity increases, and the solubility and formability are likely to decrease. On the other hand, if [Al2O3] / ([R2O]+[RO]) is too small, the liquidus temperature increases, and the liquidus viscosity is likely to decrease. Therefore, the suitable lower limit range of [Al2O3] / ([R2O]+[RO]) is 0.2 or more, 0.25 or more, 0.3 or more, 0.35 or more, and particularly 0.4 or more. It should be noted that the molar ratio [Al2O3] / ([R2O]+[RO]) refers to the value obtained by dividing the Al2O3 content by the total amount of alkali metal oxides R2O and the total amount of alkaline earth metal oxides RO.
[0126] The suitable upper limit range of the molar ratio [Na2O] / [Li2O] is 1.0 or less, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, 0.35 or less, particularly 0.3 or less. If the molar ratio [Na2O] / [Li2O] is too large, the efficiency of ion exchange between Li ions contained in the glass and Na ions in the molten salt tends to decrease. On the other hand, if the molar ratio [Na2O] / [Li2O] is too small, the efficiency of ion exchange between Na ions contained in the glass and K ions in the molten salt tends to decrease. It is preferably 0.03 or more, 0.05 or more, 0.07 or more, 0.10 or more, 0.15 or more, particularly 0.2 or more. It should be noted that the molar ratio [Na2O] / [Li2O] is the value obtained by dividing the content of Na2O by the content of Li2O.
[0127] The suitable lower limit range of the molar ratio ([ZnO]+[Li2O]+[Na2O]+[K2O]) / [Al2O3] is 0.7 or more, 0.75 or more, 0.8 or more, 0.85 or more, 0.9 or more, particularly 0.95 or more. If the molar ratio ([ZnO]+[Li2O]+[Na2O]+[K2O]) / [Al2O3] is too small, the efficiency of ion exchange tends to decrease, and it is difficult to lower the softening point. On the other hand, even if the molar ratio ([ZnO]+[Li2O]+[Na2O]+[K2O]) / [Al2O3] is too large, the efficiency of ion exchange also tends to decrease. Therefore, the suitable upper limit range of the molar ratio ([ZnO]+[Li2O]+[Na2O]+[K2O]) / [Al2O3] is 2 or less, 1.8 or less, 1.9 or less, 1.8 or less, 1.7 or less, 1.6 or less, 1.5 or less, 1.4 or less, particularly 1.3 or less. It should be noted that the molar ratio ([ZnO]+[Li2O]+[Na2O]+[K2O]) / [Al2O3] is the value obtained by dividing the total amount of the contents of ZnO, Li2O, Na2O and K2O by Al2O3.
[0128] The molar ratio [MgO] / [Al2O3] is preferably 1.0 or less, 0.8 or less, 0.6 or less, 0.5 or less, 0.4 or less, 0.3 or less, 0.25 or less, particularly preferably 0.2 or less. If [MgO] / [Al2O3] is too large, reaction products (Japanese original: 反応ブツ) tend to be generated when contacting with the formed body (particularly alumina formed body) at high temperature, and the quality of the plate-shaped formed glass may be reduced. On the other hand, the lower limit of [MgO] / [Al2O3] is not particularly limited, for example, it is 0% or more, 0.01 or more, 0.03 or more, 0.05 or more. It should be noted that "[MgO] / [Al2O3]" is the value obtained by dividing the content of MgO by the content of Al2O3.
[0129] If the range of the molar ratio ([SiO2] + [B2O3] + [P2O5]) / ((100 × [SnO2]) × ([Li2O] + [Na2O] + [K2O] + [MgO] + [CaO] + [BaO] + [SrO] + [ZnO] + [Al2O3])) is limited, it is possible to improve the clarity and the resistance to devitrification. The suitable lower limit range of the molar ratio ([SiO2] + [B2O3] + [P2O5]) / ((100 × [SnO2]) × ([Li2O] + [Na2O] + [K2O] + [MgO] + [CaO] + [BaO] + [SrO] + [ZnO] + [Al2O3])) is above 0.30, above 0.33, above 0.35, above 0.37, above 0.38, above 0.39, above 0.40, above 0.41, above 0.42, above 0.43, above 0.44, above 0.45, above 0.48, above 0.50, above 0.51, above 0.52, above 0.53, above 0.54, and especially above 0.55. If the molar ratio ([SiO2] + [B2O3] + [P2O5]) / ((100 × [SnO2]) × ([Li2O] + [Na2O] + [K2O] + [MgO] + [CaO] + [BaO] + [SrO] + [ZnO] + [Al2O3])) is too small, SnO2 crystals are easily precipitated. The upper limit range of the molar ratio ([SiO2] + [B2O3] + [P2O5]) / ((100 × [SnO2]) × ([Li2O] + [Na2O] + [K2O] + [MgO] + [CaO] + [BaO] + [SrO] + [ZnO] + [Al2O3])) is not particularly limited, for example, 4.0 or less, 3.0 or less, 2.0 or less, 1.5 or less, or 1.0 or less. It should be noted that "([SiO2]+[B2O3]+[P2O5]) / ((100×[SnO2])×([Al2O3]+[Li2O]+[Na2O]+[K2O]+[MgO]+[CaO]+[BaO]+[SrO]+[ZnO]))" is the value obtained by dividing the total amount of SiO2, B2O3 and P2O5 by 100 times the content of SnO2 and multiplying the total amount of Al2O3, Li2O, Na2O, K2O, MgO, CaO, BaO, SrO and ZnO.
[0130] The suitable lower limit range of the molar ratio [Li2O] / ([Na2O]+[K2O]) is 0.1 or more, 0.3 or more, 0.5 or more, 0.6 or more, and especially 0.7 or more. If the molar ratio [Li2O] / ([Na2O]+[K2O]) is too small, it is possible that the ion exchange performance cannot be fully exerted, and in particular, the efficiency of the ion exchange between the Li ions contained in the glass and the Na ions in the molten salt is easily reduced. On the other hand, if [Li2O] / ([Na2O]+[K2O]) is too large, it is easy to precipitate devitrified crystals on the glass, and it is difficult to form it into a plate shape using an overflow down-drawing method or the like. Therefore, the suitable upper limit range of [Li2O] / ([Na2O]+[K2O]) is 10 or less, 9 or less, 8.5 or less, 8 or less, 7.5 or less, 7 or less, 6.5 or less, 6.3 or less, and especially 6 or less. It should be noted that “[Li2O] / ([Na2O]+[K2O])” refers to a value obtained by dividing the content of Li2O by the total amount of Na2O and K2O.
[0131] The following formula Q value is a factor related to acid resistance. If the Q value is too small, acid resistance is easily reduced. Therefore, the applicable lower limit of the Q value is more than -30, more than -25, more than -20, more than -18, more than -15, more than -12, more than -10, more than -8, particularly more than -5. On the other hand, if the Q value is too large, it is possible to fail to give full play to the ion exchange performance. Therefore, the applicable upper limit of the Q value is less than 50, less than 45, less than 42, less than 40, particularly less than 35.
[0132] Q=[SiO2]+1.2×[P2O5]-3×[Al2O3]-[B2O3]-2×[Li2O]-1.5×[Na2O]-[K2O]
[0133] The suitable lower limit range of the molar ratio [Li2O] / [Al2O3] is 0.1 or more, 0.2 or more, 0.3 or more, 0.40 or more, 0.42 or more, 0.44 or more, 0.50 or more, 0.52 or more, 0.55 or more, and especially 0.58 or more. If the molar ratio [Li2O] / [Al2O3] is too small, it is possible that the ion exchange performance cannot be fully exerted, and the efficiency of the ion exchange between the Li ions contained in the glass and the Na ions in the molten salt is easily reduced. On the other hand, if [Li2O] / [Al2O3] is too large, it is easy to precipitate devitrified crystals on the glass, and it is difficult to form into a plate shape by overflow down-drawing method, etc. Therefore, the suitable upper limit range of [Li2O] / [Al2O3] is 2.0 or less, 1.8 or less, 1.5 or less, 1.2 or less, 1.0 or less, 0.8 or less, 0.7 or less, 0.68 or less, and especially 0.60 or less. It should be noted that “[Li 2 O] / [Al 2 O 3 ]” refers to a value obtained by dividing the content of Li 2 O by the content of Al 2 O 3 .
[0134] The X value in the following formula is a factor related to the exchange rate of Li ions and Na ions. If the X value is too small, the efficiency of the ion exchange between Li ions and Na ions in the molten salt is reduced, and it is difficult to generate compressive stress. In particular, the stress depth (DOC) of the compressive stress layer in the ion exchange between Li ions contained in the glass and Na ions in the molten salt is Na ) may become smaller. Therefore, the suitable lower limit range of the X value is 300 or more, 320 or more, 330 or more, 340 or more, 350 or more, 400 or more, 450 or more, 460 or more, 48 or more, 500 or more, 520 or more, and particularly 550 or more. The upper limit range of X is not particularly limited, and is, for example, 900 or less, 880 or less.
[0135] X=-1.49×[SiO2]+26.98×[Al2O3]-3.23×[B2O3]+48.56×[Li2O]-24.31×[Na2O]-0.28×[MgO]+2.74×[CaO]
[0136] The Y value in the following formula is a factor related to the exchange rate of Na ions and K ions. If the Y value is too small, the efficiency of the ion exchange between the Na ions contained in the glass and the K ions in the molten salt is reduced, and it is difficult to generate compressive stress. In particular, the stress depth (DOL) of the compressive stress layer in the ion exchange between the Na ions contained in the glass and the K ions in the molten salt is K) may become smaller. Therefore, the suitable lower limit range of the Y value is 4 or more, 4.3 or more, 4.5 or more, 4.8 or more, 5 or more, 5.2 or more, 5.5 or more, 6 or more, 7 or more, 8 or more, 9 or more, 10 or more, and particularly 11 or more. The upper limit range of the Y value is not particularly limited, and is, for example, 30 or less, 25 or less.
[0137] Y=3+0.21×[SiO2]+0.25×[Al2O3]-0.33×[B2O3]-0.55×[Li2O]+0.45×[Na2O]-0.97×[MgO]-1.46×[CaO]
[0138] The following formula Z value has a strong correlation with the exchange rate of Li ions and Na ions and the exchange rate of Na ions and K ions, which is a particularly important factor when multiple ion exchange treatments are performed on the strengthening glass plate. If the Z value is too small, the efficiency of the ion exchange between Li ions and Na ions in the molten salt is easily reduced, and the efficiency of the ion exchange between Na ions and K ions in the molten salt is also easily reduced. Therefore, it is difficult to generate compressive stress in both of the above-mentioned ion exchanges. Therefore, the suitable lower limit range of the Z value is more than 18, more than 18.5, more than 19, more than 20, more than 25, more than 30, more than 35, more than 45, and especially more than 50. The upper limit range of the Z value is not particularly limited, for example, less than 120, less than 100.
[0139] Z=0.13×[SiO2]+2.36×[Al2O3]-0.14×[B2O3]+4.90×[Li2O]-5.53×[Na2O]-2.14×[MgO]-2.34×[CaO]
[0140] The W value in the following formula is a factor related to Young's modulus. If the W value is too small, the Young's modulus becomes low and the glass is easily broken. Therefore, the suitable lower limit range of the W value is 250 or more, 300 or more, 330 or more, 340 or more, 350 or more, 360 or more, 370 or more, 400 or more, 430 or more, 450 or more, 480 or more, and particularly 500 or more. The upper limit range of the W value is not particularly limited, for example, 750 or less, 700 or less.
[0141] W=0.07×[SiO2]+18.17×[Al2O3]-4.42×[B2O3]+41.43×[Li2O]-29.30×[Na2O]+1.43×[MgO]-10.43×[CaO]
[0142] The U value in the following formula is a factor related to fracture toughness. If the U value is too small, the fracture toughness value becomes low and the glass is easily broken. Therefore, the suitable lower limit range of the U value is 7000 or more, 7100 or more, 7500 or more, 7600 or more, 7700 or more, 7750 or more, 7800 or more, 7850 or more, and particularly 7900 or more. The upper limit range of the U value is not particularly limited, for example, 20000 or less, 18000 or less, 15000 or less, 12000 or less, 10000 or less, and 9500 or less.
[0143] U=87.39×[SiO2]+180.12×[Al2O3]+93.63×[B2O3]+113.78×([MgO]+[CaO]+[BaO]+[SrO])-46.2×[Li2O]-71.1×[Na2O]-58.6×[K2O]-40.0×[P2O5]
[0144] In addition to the above-mentioned components, for example, the following components may be added.
[0145] TiO2 is a component that improves ion exchange performance and reduces high temperature viscosity, but if its content is too much, transparency and resistance to devitrification are easily reduced. Therefore, the suitable content of TiO2 is 0-10%, 0-5%, 0-3%, 0-1.5%, 0-1%, 0-0.1%, and particularly 0.001-0.1%.
[0146] ZrO2 is a component that increases Vickers hardness and increases viscosity and strain point near liquidus viscosity, but if its content is too much, the devitrification resistance may be significantly reduced. Therefore, the suitable content of ZrO2 is 0-10%, 0-5%, 0-3%, 0-1.5%, 0-1%, 0-0.5%, 0-0.4%, 0-0.3%, 0-0.2%, and particularly 0-0.1%.
[0147] La2O3 is a component that improves Young's modulus and fracture toughness, but if its content is too much, the liquid phase viscosity may decrease. Therefore, the suitable content of La2O3 is 0-5%, 0-3%, 0-1.5%, 0-1%, 0-0.8%, 0-0.5%, 0-0.4%, 0-0.3%, 0-0.2%, and especially 0-0.1%.
[0148] Fe2O3 is an impurity mixed from the raw material. The suitable upper limit range of Fe2O3 is less than 0.1%, less than 0.08%, less than 0.05%, less than 0.02%, less than 0.015%, less than 0.01%, less than 0.008%, and especially less than 0.005%. If the content of Fe2O3 is too much, the transmittance of the protective glass is easily reduced. On the other hand, the suitable lower limit range is more than 0.001%, more than 0.002%, and more than 0.003%. If the content of Fe2O3 is too little, the raw material cost is high due to the use of high-purity raw materials, and the product cannot be manufactured cheaply.
[0149] As a clarifier, 0.001 to 1% of SO3 and / or CeO2 may be added.
[0150] Rare earth oxides such as Nd2O3, Y2O3, Nb2O5, Ta2O5, and Hf2O3 are components that increase the Young's modulus. However, the raw material cost is high, and if a large amount is added, the devitrification resistance is easily reduced. Therefore, the suitable total amount of rare earth oxides is 5% or less, 4% or less, 3% or less, 2% or less, 1% or less, 0.5% or less, and especially 0.1% or less, and the suitable contents of Nd2O3, Y2O3, Nb2O5, Ta2O5, and Hf2O3 are respectively 3% or less, 2% or less, 1% or less, 0.5% or less, and especially 0.1% or less.
[0151] In the tempered glass plate and tempered glass plate of the present invention, it is preferred that the glass composition substantially does not contain As2O3, Sb2O3, PbO and F from an environmental perspective. In addition, it is also preferred that Bi2O3 is substantially not contained from an environmental perspective. "Substantially not containing" means that the indicated component is not actively added as a glass component, but the addition of an impurity level is allowed, and specifically, it means that the content of the indicated component is less than 0.05%.
[0152] The tempered glass plate and tempered glass plate of the present invention preferably have the following properties.
[0153] The density (ρ) is preferably 2.55 g / cm 3 Below, 2.53g / cm 3 Below, 2.50g / cm 3 Below, 2.49g / cm 3 Below, 2.48g / cm 3 Below, 2.45g / cm 3 Below, 2.35~2.44g / cm 3 , especially 2.25~2.44g / cm 3 The lower the density, the lighter the tempered glass sheet can be.
[0154] Thermal expansion coefficient (α) at 30-380°C 30-380℃ ) is preferably 150×10 -7 / ℃ below, 100×10 -7 / ℃ below, 50~95×10 -7 / ℃、40~85×10 -7 / °C, particularly preferably 35 to 80×10 -7 / °C. In addition, the "thermal expansion coefficient at 30 to 380°C" refers to a value obtained by measuring an average thermal expansion coefficient using a dilatometer.
[0155] The softening point (Ts) is preferably 950° C. or less, 940° C. or less, 930° C. or less, 920° C. or less, 910° C. or less, 900° C. or less, 890° C. or less, 880° C. or less, 870° C. or less, 860° C. or less, 850° C. or less, 840° C. or less, 830° C. or less, 820° C. or less, 810° C. or less, and particularly preferably 700 to 800° C. If the softening point is too high, hot workability may be reduced.
[0156] High temperature viscosity 10 2.5 dPa·s at temperature (10 2.5 dPa·s) is preferably 1680°C or less, 1670°C or less, 1660°C or less, 1650°C or less, 1640°C or less, 1630°C or less, 1620°C or less, 1600°C or less, 1550°C or less, 1520°C or less, 1500°C or less, and particularly preferably 1300 to 1490°C. If the high temperature viscosity is 10 2.5 If the temperature at dPa·s is too high, the meltability and formability will be reduced, and it will be difficult to form the molten glass into a sheet shape.
[0157] The liquid phase viscosity is preferably 10 3.74 dPa·s or more, 10 4.3 dPa·s or more, 10 4.4 dPa·s or more, 10 4.5 dPa·s or more, 10 4.6 dPa·s or more, 10 4.7 dPa·s or more, 10 4.8 dPa·s or more, 10 4.9 dPa·s or more, 10 5.0 dPa·s or more, 10 5.1 dPa·s or more, 10 5.2 dPa·s or more, 10 5.3 dPa·s or more, 10 5.4 dPa·s or more, particularly preferably 10 5.5dPa·s or more. It should be noted that the higher the liquidus viscosity, the higher the devitrification resistance, and the less likely devitrified products are to be produced during molding. Here, "liquidus viscosity" refers to the value obtained by measuring the viscosity at the liquidus temperature using a platinum ball pulling method.
[0158] Young's modulus (E) is preferably 60 GPa or more, 65 GPa or more, 70 GPa or more, 71 GPa or more, 72 GPa or more, 73 GPa or more, 74 GPa or more, and particularly preferably 75 GPa or more. If the Young's modulus is low, the protective glass is easily bent when the plate thickness is thin. In addition, the upper limit range of the Young's modulus is not particularly limited, and is substantially below 100 GPa. It should be noted that the "Young's modulus" can be calculated by a known resonance method.
[0159] The tempered glass plate of the present invention has a compressive stress layer on the surface. The compressive stress value (CS) of the outermost surface of the tempered glass plate is preferably 200 MPa or more, 220 MPa or more, 250 MPa or more, 280 MPa or more, 300 MPa or more, 310 MPa or more, 320 MPa or more, 330 MPa or more, 340 MPa or more, 350 MPa or more, 360 MPa or more, 370 MPa or more, 380 MPa or more, 390 MPa or more, 400 MPa or more, 420 MPa or more, 430 MPa or more, and particularly preferably 450 MPa or more. The larger the compressive stress value (CS) of the outermost surface, the higher the Vickers hardness. On the other hand, if a very large compressive stress is formed on the surface, the tensile stress inherent in the tempered glass plate becomes extremely high, and the dimensional change before and after the ion exchange treatment may become large. Therefore, the compressive stress value (CS) of the outermost surface is preferably below 1400MPa, below 1200MPa, below 1100MPa, below 1000MPa, below 900MPa, below 700MPa, below 680MPa, below 650MPa, and particularly preferably below 600MPa. It should be noted that if the ion exchange time is shortened or the temperature of the ion exchange solution is lowered, there is a tendency for the compressive stress value of the outermost surface to increase.
[0160] The compressive stress value (CS30) of the tempered glass plate at a depth of 30 μm from the outermost surface is preferably 35 MPa or more, 40 MPa or more, 50 MPa or more, 60 MPa or more, 70 MPa or more, 80 MPa or more, 90 MPa or more, 100 MPa or more, 105 MPa or more, 110 MPa or more, 115 MPa or more, and particularly preferably 120 MPa or more. The greater the compressive stress value (CS30) at a depth of 30 μm from the outermost surface, the higher the strength. On the other hand, if a very large compressive stress is formed at a depth of 30 μm from the outermost surface, the inherent tensile stress in the tempered glass plate becomes extremely high, and the dimensional change before and after the ion exchange treatment may become large. Therefore, the compressive stress value (CS30) at a depth of 30 μm from the outermost surface is preferably 400 MPa or less, 350 MPa or less, 300 MPa or less, 250 MPa or less, 230 MPa or less, 220 MPa or less, 210 MPa or less, 205 MPa or less, 200 MPa or less, 195 MPa or less, and particularly preferably 190 MPa or less.
[0161] The compressive stress value (CS50) of the tempered glass plate at a depth of 50 μm from the outermost surface is preferably 20 MPa or more, 30 MPa or more, 40 MPa or more, 50 MPa or more, 60 MPa or more, 70 MPa or more, 80 MPa or more, 90 MPa or more, 95 MPa or more, and particularly preferably 100 MPa or more. The greater the compressive stress value (CS50) at a depth of 50 μm from the outermost surface, the higher the strength. On the other hand, if a very large compressive stress is formed at a depth of 50 μm from the outermost surface, the inherent tensile stress in the tempered glass plate becomes extremely high, and the dimensional change before and after the ion exchange treatment may become large. Therefore, the compressive stress value (CS50) at a depth of 50 μm from the outermost surface is preferably 380 MPa or less, 350 MPa or less, 300 MPa or less, 250 MPa or less, 220 MPa or less, 210 MPa or less, 200 MPa or less, 195 MPa or less, 2190 MPa or less, 180 MPa or less, and particularly preferably 170 MPa or less.
[0162] The internal tensile stress value (CT) of the tempered glass plate is preferably 150 MPa or less, 130 MPa or less, 120 MPa or less, 110 MPa or less, 100 MPa or less, 90 MPa or less, 85 MPa or less, 80 MPa or less, 75 MPa or less, 70 MPa or less, 60 MPa or less, and particularly preferably 50 MPa or less. If the internal tensile stress value is too large, the tempered glass plate may self-destruct due to point collision. The upper limit range of the internal tensile stress value (CT) is not particularly limited, but is substantially 5 μm or more.
[0163] The stress depth of the compressive stress layer of the tempered glass plate, that is, the depth (DOC) at which the stress value is zero, is preferably 3 μm or more, 5 μm or more, 10 μm or more, 20 μm or more, 30 μm or more, 40 μm or more, 45 μm or more, 50 μm or more, 55 μm or more, 58 μm or more, 60 μm or more, 65 μm or more, 70 μm or more, 75 μm or more, 80 μm or more, 85 μm or more, and particularly preferably 90 μm or more. The deeper the stress depth, the more difficult it is for the protrusions and sand particles on the road surface to reach the tensile stress layer when the smartphone falls, which can reduce the probability of damage to the protective glass. On the other hand, if the stress depth is too deep, the dimensional change before and after the ion exchange treatment may become larger. In addition, there is a trend that the compressive stress value of the outermost surface decreases. Therefore, the stress depth (DOC) is preferably 200 μm or less, 180 μm or less, 150 μm or less, 140 μm or less, 135 μm or less, 130 μm or less, 125 μm or less, particularly preferably 120 μm or less, particularly preferably 110 μm or less. It should be noted that if the ion exchange time is extended or the temperature of the ion exchange solution is increased, there is a tendency for the stress depth to become deeper.
[0164] In addition, when the tempered glass plate was immersed in a KNO3 molten salt at 430°C for 4 hours to perform an ion exchange treatment, the compressive stress value (CS) of the outermost surface during the ion exchange between Na ions contained in the glass and K ions in the molten salt was K ) is preferably 200 MPa or more, 220 MPa or more, 250 MPa or more, 280 MPa or more, 300 MPa or more, 310 MPa or more, 320 MPa or more, 330 MPa or more, 340 MPa or more, 350 MPa or more, 360 MPa or more, 370 MPa or more, 380 MPa or more, 390 MPa or more, 400 MPa or more, 420 MPa or more, 430 MPa or more, and particularly preferably 450 MPa or more. The larger the compressive stress value of the outermost surface, the higher the Vickers hardness. On the other hand, if extremely large compressive stress is formed on the surface, the inherent tensile stress in the tempered glass plate becomes extremely high, and the dimensional change before and after the ion exchange treatment may become large. Therefore, the compressive stress value (CS) of the outermost surface is preferably 200 MPa or more, 220 MPa or more, 250 MPa or more, 280 MPa or more, 300 MPa or more, 310 MPa or more, 320 MPa or more, 330 MPa or more, 340 MPa or more, 350 MPa or more, 360 MPa or more, 370 MPa or more, 380 MPa or more, 390 MPa or more, 400 MPa or more, 420 MPa or more, 430 MPa or more, and particularly preferably 450 MPa or more. The larger the compressive stress value of the outermost surface, the higher the Vickers hardness. On the other hand, if extremely large compressive stress is formed on the surface, the tensile stress inherent in the tempered glass plate becomes extremely high, and the dimensional change before and after the ion exchange treatment may become large. K ) is preferably below 1400MPa, below 1200MPa, below 1100MPa, below 1000MPa, below 900MPa, below 700MPa, below 680MPa, below 650MPa, and particularly preferably below 600MPa. It should be noted that if the ion exchange time is shortened or the temperature of the ion exchange solution is reduced, there is a trend that the compressive stress value on the outermost surface becomes larger.
[0165] When the tempered glass plate is immersed in a KNO3 molten salt at 430°C for 4 hours to perform an ion exchange treatment, the stress depth (DOL) in the ion exchange between the Na ions contained in the glass and the K ions in the molten salt is K ) is preferably 3μm or more, 4μm or more, 4.5μm or more, 5μm or more, 6μm or more, 7μm or more, 8μm or more, 9μm or more, and particularly preferably 10μm or more. The deeper the stress depth, the more difficult it is for protrusions and sand on the road surface to reach the tensile stress layer when the smartphone falls, which can reduce the probability of damage to the protective glass. On the other hand, if the stress depth is too deep, the dimensional change before and after the ion exchange treatment may become larger. In addition, there is a trend for the compressive stress value of the outermost surface to decrease. Therefore, the stress depth (DOL K ) is preferably 40 μm or less, 35 μm or less, 30 μm or less, 28 μm or less, 25 μm or less, 23 μm or less, 20 μm or less, and particularly preferably 18 μm or less. It should be noted that if the ion exchange time is extended or the temperature of the ion exchange solution is increased, there is a tendency for the stress depth to become deeper.
[0166] In addition, when the tempered glass plate was immersed in a NaNO3 molten salt at 380°C for 1 hour to perform an ion exchange treatment, the compressive stress value (CS) of the outermost surface during the ion exchange between Li ions contained in the glass and Na ions in the molten salt was Na ) is preferably 140 MPa or more, 150 MPa or more, 160 MPa or more, 170 MPa or more, 180 MPa or more, 190 MPa or more, and particularly preferably 200 MPa or more. The greater the compressive stress value of the outermost surface, the higher the strength. On the other hand, if a very large compressive stress is formed on the surface, the inherent tensile stress in the tempered glass sheet becomes extremely high, and the dimensional change before and after the ion exchange treatment may become large. Therefore, the compressive stress value (CS) of the outermost surface is preferably 140 MPa or more, 150 MPa or more, 160 MPa or more, 170 MPa or more, 180 MPa or more, 190 MPa or more, and particularly preferably 200 MPa or more. The greater the compressive stress value of the outermost surface, the higher the strength. On the other hand, if a very large compressive stress is formed on the surface, the inherent tensile stress in the tempered glass sheet becomes extremely high, and the dimensional change before and after the ion exchange treatment may become large. Na ) is preferably 650 MPa or less, 630 MPa or less, 600 MPa or less, 580 MPa or less, 560 MPa or less, 550 MPa or less, 540 MPa or less, 530 MPa or less, 500 MPa or less, 480 MPa or less, 450 MPa or less, 430 MPa or less, 400 MPa or less, 380 MPa or less, and particularly preferably 350 MPa or less.
[0167] When the tempered glass plate is immersed in a molten salt of NaNO3 at 380°C for 1 hour to perform an ion exchange treatment, the compressive stress value (CS30 Na) is preferably 35 MPa or more, 40 MPa or more, 50 MPa or more, 60 MPa or more, 70 MPa or more, 80 MPa or more, 90 MPa or more, 100 MPa or more, 105 MPa or more, 110 MPa or more, 115 MPa or more, and particularly preferably 120 MPa or more. The compressive stress value (CS30 Na ) is larger, the higher the strength is. On the other hand, if a large compressive stress is formed at a depth of 30 μm from the outermost surface, the inherent tensile stress in the tempered glass plate becomes extremely high, and the dimensional change before and after the ion exchange treatment may become larger. Therefore, the compressive stress value at a depth of 30 μm from the outermost surface (CS30 Na ) is preferably 400 MPa or less, 350 MPa or less, 300 MPa or less, 250 MPa or less, 230 MPa or less, 220 MPa or less, 210 MPa or less, 205 MPa or less, 200 MPa or less, 195 MPa or less, and particularly preferably 190 MPa or less.
[0168] When the tempered glass plate is immersed in a molten salt of NaNO3 at 380°C for 1 hour to perform an ion exchange treatment, the stress depth (DOC) in the ion exchange between the Li ions contained in the glass and the Na ions in the molten salt is Na ) is preferably 3μm or more, 5μm or more, 10μm or more, 20μm or more, 30μm or more, 40μm or more, 45μm or more, 50μm or more, 55μm or more, 58μm or more, 60μm or more, 65μm or more, 70μm or more, 75μm or more, 80μm or more, 85μm or more, and particularly preferably 90μm or more. The deeper the stress depth, the more difficult it is for protrusions and sand on the road surface to reach the tensile stress layer when the smartphone falls, which can reduce the probability of damage to the protective glass. On the other hand, if the stress depth is too deep, the dimensional change before and after the ion exchange treatment may become larger. In addition, there is a tendency for the compressive stress value of the outermost surface to decrease. Therefore, the stress depth (DOC Na ) is preferably 200 μm or less, 180 μm or less, 150 μm or less, 140 μm or less, 130 μm or less, 120 μm or less, and particularly preferably 110 μm or less. It should be noted that if the ion exchange time is extended or the temperature of the ion exchange solution is increased, there is a tendency for the stress depth to become deeper.
[0169] When the tempered glass plate is immersed in a NaNO3 molten salt at 380°C for 1 hour to perform an ion exchange treatment, the internal tensile stress value (CTcv) during the ion exchange between the Li ions contained in the glass and the Na ions in the molten salt is Na) is preferably 150 MPa or less, 130 MPa or less, 120 MPa or less, 110 MPa or less, 100 MPa or less, 90 MPa or less, 85 MPa or less, 80 MPa or less, 75 MPa or less, 70 MPa or less, 60 MPa or less, and particularly preferably 50 MPa or less. If the internal tensile stress value is too large, the tempered glass sheet may self-destruct due to point collision. Internal tensile stress value (CTcv Na ) is not particularly limited, but is substantially greater than 5 μm.
[0170] When the tempered glass plate is immersed in a molten salt of NaNO3 at 380°C for 1 hour to perform an ion exchange treatment, the stress depth (DOC) in the ion exchange between the Li ions contained in the glass and the Na ions in the molten salt is Na ) and the stress depth (DOL) in the ion exchange between Na ions contained in the glass and K ions in the molten salt when the tempered glass plate is immersed in a KNO3 molten salt at 430°C for 4 hours for ion exchange treatment. K ) is the ratio of DOC Na / DOL K Preferably, it is 15 or less, 12 or less, 10 or less, 9 or less, 8 or less, 7.5 or less, 7.0 or less, 6.5 or less, 6.0 or less, 5.5 or less, 5.0 or less, or 4.5 or less. If DOC Na / DOL K If the DOC is too large, the compressive stress value (CS30) at a depth of 30 μm from the outermost surface of the tempered glass plate subjected to two-stage tempering may become smaller when the glass plate is immersed in a NaNO3 molten salt and then immersed in a KNO3 molten salt. Na / DOL K If the value is too small, the time required for ion exchange between Li ions contained in the glass and Na ions in the molten salt may become too long.
[0171] In the tempered glass plate of the present invention, the mass loss per unit surface area when immersed in a 5 mass % HCl aqueous solution heated to 80° C. for 24 hours is preferably 2.0 mg / cm 2 Below, 1.5mg / cm 2 Below, 1.0mg / cm 2 Below, 0.8mg / cm 2 Below, particularly preferably 0.5 mg / cm 2 The tempered glass plate may come into contact with an acidic chemical solution depending on the use environment of the device, and from the viewpoint of preventing malfunction of the device, it is preferred that the acid resistance is high.
[0172] The mass loss per unit surface area when immersed in a 5 mass % NaOH aqueous solution heated to 80° C. for 6 hours is preferably 5.0 mg / cm 2 Below, 4.5mg / cm 2 Below, 4.0mg / cm 2 Below, 3.5mg / cm 2 Below, 3.0mg / cm 2 Below, particularly preferably 2.0 mg / cm 2 The tempered glass plate may come into contact with alkaline chemicals or detergents depending on the use environment of the device, and therefore is required to have high alkali resistance.
[0173] The fracture toughness K1c is preferably 0.75 MPa·m 0.5 Above, 0.78MPa·m 0.5 Above, 0.79MPa·m 0.5 Above, 0.80MPa·m 0.5 Above, 0.81MPa·m 0.5 Above, particularly preferably 0.82 MPa·m 0.5 If the fracture toughness K1c is low, the tempered glass plate is easily broken. It should be noted that the upper limit of the fracture toughness is not particularly limited, but is realistically 10 MPa·m 0.5 the following.
[0174] The fracture energy γ is the energy consumed per unit fracture area during fracture, which is given by γ = (K1c) 2 The energy of fracture γ is preferably 5.0 J / m 2 Above, 5.5J / m 2 Above, 6.0J / m 2 Above, 6.5J / m 2 Above, 7.0J / m 2 Above, 7.5J / m 2 Above, 7.8J / m 2 More than, particularly preferably 8.0 J / m 2 If the fracture energy γ is low, the tempered glass sheet is easily shattered when broken, making it difficult to ensure safety. It should be noted that the upper limit of the fracture energy is not particularly limited, but is realistically 30 J / m 2 the following.
[0175] The 4-point bending strength after damage of the tempered glass plate of the present invention is preferably 150MPa or more, 160MPa or more, 1170MPa or more, 175MPa or more, 180MPa or more, 185MPa or more, 190MPa or more, 195MPa or more, and particularly preferably 200MPa or more. If the 4-point bending strength after damage is too low, it is easy to break when it is used as a protective glass for a smartphone. It should be noted that the upper limit of the 4-point bending strength after damage is not particularly limited, and is realistically 1500MPa or less.
[0176] In the tempered glass plate of the present invention, the plate thickness is preferably 2.0 mm or less, 1.5 mm or less, 1.3 mm or less, 1.1 mm or less, 1.0 mm or less, 0.9 mm or less, and particularly preferably 0.8 mm or less. The smaller the plate thickness, the lower the quality of the tempered glass plate. On the other hand, if the plate thickness is too thin, it is difficult to obtain the desired mechanical strength. Therefore, the plate thickness is preferably 0.03 mm or more, 0.05 mm or more, 0.1 mm or more, 0.2 mm or more, 0.3 mm or more, 0.4 mm or more, 0.5 mm or more, 0.6 mm or more, and particularly preferably 0.7 mm or more.
[0177] The method for producing a tempered glass plate of the present invention is characterized by comprising the following steps: a preparation step of preparing the tempered glass plate, wherein the tempered glass plate contains, as a glass composition, SiO2 50-80%, Al2O3 7-25%, B2O3 0-15%, Li2O 0-15%, Na2O 0-25%, K2O 0-10%, MgO 0-15%, CaO 0-10%, BaO 0-10%, SrO 0-10%, ZnO 0-10%, P2O5 0-15%, TiO2 0-10%, ZrO2 0-10%, SnO2 0 to 0.30%, [B2O3] + [MgO] + [CaO] is 0.1 to 30%, and ([Li2O] + [Na2O] + [K2O]) / [Al2O3] is 0.5 to 2.0; and an ion exchange step, wherein the strengthened glass plate is subjected to ion exchange treatment to obtain a strengthened glass plate having a compressive stress layer on the surface. It should be noted that the method for manufacturing a strengthened glass plate of the present invention includes not only a case where multiple ion exchange treatments are performed, but also a case where only one ion exchange treatment is performed.
[0178] The method for manufacturing tempered glass is as follows. Preferably, first, glass raw materials prepared in a manner to obtain a desired glass composition are placed in a continuous melting furnace, heated and melted at 1400 to 1700°C, clarified, and then the molten glass is supplied to a forming device, formed into a plate shape, and cooled. After forming into a plate shape, the method of cutting into a predetermined size can be a known method.
[0179] As a method for forming molten glass into a plate-like shape, an overflow down-draw method is preferred. In the overflow down-draw method, there is an overflow confluence surface parallel to the main surface inside, and the surface of the glass sheet that should become the surface does not contact the surface of the forming body refractory, and is formed into a plate-like shape in the state of a free surface. Therefore, it is possible to manufacture a glass sheet with good surface quality although it is not ground inexpensively. In addition, in the overflow down-draw method, as the forming body refractory, an alumina refractory, a zirconium refractory, and a zirconium oxide refractory can be used. And the tempered glass plate of the present invention and the tempered glass plate have good compatibility with alumina refractory, zirconium oxide refractory (particularly alumina refractory), so they have properties that are not easy to react with these refractory materials and produce bubbles, foreign matter (Japanese original: ブツ), etc.
[0180] In addition to the overflow down-draw method, various forming methods can be used, such as the float method, the down-draw method (slot down-draw method, re-draw method, etc.), the roll method (Japanese original: Roll-A-Wut method), the pressing method, and the like.
[0181] When forming the molten glass, it is preferred to cool the molten glass at a cooling rate of 3°C / min or more and less than 1000°C / min in the temperature range between the annealing point and the strain point of the molten glass. The lower limit of the cooling rate is preferably 10°C / min or more, 20°C / min or more, 30°C / min or more, and particularly preferably 50°C / min or more, and the upper limit is preferably less than 1000°C / min, less than 500°C / min, and particularly preferably less than 300°C / min. If the cooling rate is too fast, the structure of the glass becomes rough, and it is difficult to increase the Vickers hardness after the ion exchange treatment. On the other hand, if the cooling rate is too slow, the production efficiency of the glass sheet is reduced.
[0182] In the manufacturing method of the tempered glass plate of the present invention, multiple ion exchange treatments may be performed. As multiple ion exchange treatments, it is preferred that the ion exchange treatment of immersion in a molten salt containing KNO3 molten salt and / or NaNO3 molten salt is followed by immersion in a molten salt containing KNO3 molten salt and / or NaNO3 molten salt. In this way, the compressive stress value of the outermost surface can be increased while ensuring a deeper stress depth.
[0183] In particular, in the method for manufacturing a tempered glass plate of the present invention, it is preferred that after the ion exchange treatment (first ion exchange step) of immersing in a NaNO3 molten salt or a mixed molten salt of NaNO3 and KNO3, the ion exchange treatment (second ion exchange step) of immersing in a mixed molten salt of KNO3 and LiNO3 is performed. Figure 1 The non-monotonic stress curve (stress distribution in the thickness direction of the glass plate) shown as an example. Figure 1 This is a schematic diagram of a stress curve obtained by measuring the stress from the surface to the depth direction in a tempered glass plate, with compressive stress as a positive number and tensile stress as a negative number. Figure 2 yes Figure 1 An enlarged view of the low compressive stress region in the stress curve shown. Specifically, a stress curve having a first peak a, a first valley b, a second peak c, and a second valley d can be formed. As a result, the probability of damage to the protective glass when the smartphone is dropped can be greatly reduced.
[0184] It should be noted that the first peak, the first valley, the second peak, and the second valley in the present invention are defined as follows. Here, a where the surface compressive stress becomes the maximum value is set as the first peak, b where the stress gradually decreases in the depth direction from the first peak and becomes the minimum value is set as the first valley, c where the compressive stress gradually increases in the depth direction from the first valley and becomes the maximum value is set as the second peak, and d where the tensile stress gradually decreases in the depth direction from the second peak and becomes the minimum value is set as the second valley.
[0185] In the first ion exchange process, the Li ions contained in the glass are ion exchanged with the Na ions in the molten salt. When NaNO3 and KNO3 are mixed with the molten salt, the Na ions contained in the glass are ion exchanged with the K ions in the molten salt. Here, the speed of the ion exchange between the Li ions contained in the glass and the Na ions in the molten salt is faster than the speed of the ion exchange between the Na ions contained in the glass and the K ions in the molten salt, and the efficiency of the ion exchange is high. In the second ion exchange process, the Na ions near the surface of the glass (the shallow area from the outermost surface to 20% of the plate thickness) are ion exchanged with the Li ions in the molten salt, and in addition, the Na ions near the surface of the glass (the shallow area from the outermost surface to 20% of the plate thickness) are ion exchanged with the K ions in the molten salt. That is, in the second ion exchange process, it is possible to introduce K ions with a large ion radius while detaching the Na ions near the surface of the glass. As a result, it is possible to increase the compressive stress value of the outermost surface while maintaining a deeper stress depth.
[0186] In the first ion exchange step, the temperature of the molten salt is preferably 360 to 400° C., and the ion exchange time is preferably 30 minutes to 10 hours. In the second ion exchange step, the temperature of the ion exchange solution is preferably 370 to 400° C., and the ion exchange time is preferably 15 minutes to 3 hours.
[0187] On the basis of forming a non-monotonic stress curve, in the mixed molten salt of NaNO3 and KNO3 used in the first ion exchange process, the concentration of NaNO3 is preferably higher than the concentration of KNO3, and in the mixed molten salt of KNO3 and LiNO3 used in the second ion exchange process, the concentration of KNO3 is preferably higher than the concentration of LiNO3.
[0188] In the NaNO3 and KNO3 mixed molten salt used in the first ion exchange step, the concentration of KNO3 is preferably 0 mass %, 0.5 mass %, 1 mass %, 5 mass %, 7 mass %, 10 mass %, 15 mass %, and particularly preferably 20 to 90 mass %. If the concentration of KNO3 is too high, the compressive stress value formed when the Li ions contained in the glass are ion exchanged with the Na ions in the molten salt may be excessively reduced. In addition, if the concentration of KNO3 is too low, it may be difficult to measure stress using a surface stress meter FSM-6000.
[0189] In the KNO3 and LiNO3 mixed molten salt used in the second ion exchange step, the concentration of LiNO3 is preferably 0 to 5 mass%, 0.1 to 3 mass%, 0.15 to 2 mass%, and particularly preferably 0.2 to 1.5 mass%. If the concentration of LiNO3 is too low, it is difficult for Na ions near the glass surface to detach. On the other hand, if the concentration of LiNO3 is too high, the compressive stress value formed by the ion exchange of Na ions near the glass surface with K ions in the molten salt may be excessively reduced.
[0190] As the molten salt used in the second ion exchange step, a molten salt containing 100% KNO3 and no LiNO3 can be used. In this case, it is easy to obtain a stress curve without the first valley b and the second peak c. Specifically, it is easy to obtain a stress curve with an inflection point e. Figure 3 Such a stress curve.
[0191] In addition, in the manufacturing method of the tempered glass plate of the present invention, an ion exchange treatment can be used in which the glass is immersed in a mixed molten salt of NaNO3 and KNO3 once and the second ion exchange step is not performed. If this ion exchange treatment is performed, a glass having an inflection point ( Figure 3If the stress curve has an inflection point e, it is easy to obtain glass with high surface compressive stress and deep stress depth. It should be noted that, for example, when the stress curve can be approximated by a broken line composed of two straight lines, the inflection point e can be obtained as a point on the stress curve at the depth of the intersection of the two straight lines (the point where the broken line is bent). The approximation of the straight line can be performed using a known method such as the least squares method.
[0192] The depth (De) of the bending point e is preferably a shallow position close to the surface. Specifically, the depth (De) of the bending point e is preferably less than 30 μm, less than 25 μm, less than 20 μm, and particularly preferably less than 18 μm from the surface. On the other hand, if the depth (De) of the bending point e is too small, when the smartphone falls, protrusions and sand on the road surface may easily reach the tensile stress layer. Therefore, the depth (De) of the bending point e is preferably more than 3 μm, more than 4 μm, more than 4.5 μm, and particularly preferably more than 5 μm. In addition, the compressive stress at the bending point is preferably more than 80 MPa, and particularly preferably more than 100 MPa.
[0193] The mutual diffusion coefficient D of Na ions (essentially Na ions and Li ions) at 380°C Na The upper limit of the suitable range is 1×10 -11 m 2 sec -1 Below, 0.8×10 -11 m 2 sec -1 Below, 0.5×10 -11 m 2 sec -1 Below, 1×10 -12 m 2 sec -1 If the mutual diffusion coefficient D Na If the value is too large, the diffusion of Na ions will be too fast, and the compressive stress value of the deeper region of the glass plate will be easily reduced. Na The lower limit of the suitable range is 1×10 -14 m 2 sec -1 Above, 0.5×10 -13 m 2 sec -1 Above, 1×10 -13 m 2 sec -1 Above, 1×10 -13 m 2 sec -1 Above, 2×10 -13m 2 sec -1 Above, 3×10 -13 m 2 sec -1 Above, 5×10 -13 m 2 sec -1 Above, especially 8×10 -13 m 2 sec -1 If the Na ion mutual diffusion coefficient D Na If the value is too small, Na ions will not diffuse easily, and it will be difficult to obtain a deep depth of compressive stress (DOC). In addition, it will be difficult to cause mutual diffusion of Na ions and Li ions, and it will be difficult to form a non-monotonic stress curve.
[0194] Mutual diffusion coefficient of K ions (essentially K ions and Na ions) at 380°C D K The upper limit of the suitable range is 1×10 -14 m 2 sec -1 Below, 0.8×10 -14 m 2 sec -1 Below, 0.5×10 -14 m 2 sec -1 Below, 1×10 -15 m 2 sec -1 Below, 0.8×10 -15 m 2 sec -1 Below, 0.5×10 -15 m 2 sec -1 Below, 0.3×10 -15 m 2 sec -1 Below, especially 0.2×10 - 15 m 2 sec -1 Below. If the K ion mutual diffusion coefficient D K If the K ion diffusion coefficient D is too large, the K ion diffusion will be too fast, and the compressive stress value of the shallower part of the glass plate will be easily reduced. K The lower limit of the suitable range is 1×10 -17 m 2 sec -1 Above, 0.5×10 -16 m 2 sec -1 Above, 1×10 -16m 2 sec -1 Above, 2×10 -16 m 2 sec -1 Above, 3×10 -16 m 2 sec -1 Above, 5×10 -16 m 2 sec -1 Above, 7×10 -16 m 2 sec -1 Above, especially 8×10 -16 m 2 sec -1 If the K ion mutual diffusion coefficient D K If it is too small, K ions will be difficult to diffuse, and the stress depth (DOL) of the compressive stress layer during K ion exchange will be K ) may become smaller.
[0195] The ratio of the mutual diffusion coefficients at 380°C is D K / D Na The suitable lower limit range of is 0.0001 or more, 0.0003 or more, 0.0005 or more, 0.0008 or more, 0.0010 or more, 0.0012 or more, 0.0013 or more, 0.0014 or more, 0.0015 or more, 0.0016 or more, 0.0017 or more, and particularly 0.0018 or more. K / D Na If the value is too small, the diffusion rate of K ions will be too slow relative to that of Na ions. Therefore, Na ions in the deep region will diffuse excessively, and the compressive stress value at a depth of 30 μm (CS30 Na ) may become lower. K / D Na The upper limit is 0.0100 or less, 0.0080 or less, 0.0050 or less, 0.0040 or less, or 0.0030 or less. K / D Na If it is too small, it will be difficult to form a non-monotonic stress curve.
[0196] For the Na ion mutual diffusion coefficient D at 380℃ NaFor example, the Na ion concentration curve (concentration distribution) in the thickness direction of a tempered glass plate that has been ion-exchanged with a molten salt of NaNO3 (100%) at 380°C can be calculated using the following mathematical formula 1. For mathematical formula 1, it is assumed that the alkali metal ions that have been ion-exchanged diffuse in the glass according to the complementary error function that is the analytical solution of the diffusion equation, and the diffusion coefficient is specified. The Na ion concentration curve can be obtained by using EPMA measurement of a cross section of a tempered glass plate. In mathematical formula 1, x represents the depth from the surface, C(x) represents the concentration at the depth x, and C min Indicates the lowest concentration, C max represents the maximum concentration, t represents the diffusion time, and D represents the mutual diffusion coefficient. Substituting the measurement result of EPMA into Mathematical Formula 1, assuming that the measurement result is fitted to the complementary error function, the mutual diffusion coefficient D can be obtained as a solution by calculation. It should be noted that the diffusion time t is substantially consistent with the ion exchange time.
[0197] [Mathematical formula 1]
[0198]
[0199] For the K ion mutual diffusion coefficient D at 380℃ K The K ion concentration curve (concentration distribution) in the thickness direction of the tempered glass plate ion-exchanged with a molten salt of KNO3 (100%) at 380°C can be calculated using the above-mentioned Mathematical Formula 1. The K ion concentration curve can be obtained by EPMA measurement of the cross section of the tempered glass plate.
[0200] The Na ion mutual diffusion coefficient D at 380℃ Na and K ion mutual diffusion coefficient D K It can be calculated based on the ion concentration curve and Mathematical Formula 1 as described above, or it can be calculated from the concentration difference before and after the heat treatment by heat treating (annealing) the tempered glass plate after ion exchange at 380° C. The heat treatment time is not particularly limited, and is 1 minute or more, 5 minutes or more, 10 minutes or more, 20 minutes or more, and particularly 30 minutes to 120 minutes.
[0201] When two-step ion exchange is performed, the compressive stress value at a depth of 30 μm after the second ion exchange (CS30 2nd ) is lower than the compressive stress value at a depth of 30 μm after the first ion exchange (CS30 1st The compressive stress reduction rate at a depth of 30 μm before and after the second ion exchange (CS30 Droprate ) is represented by the following mathematical formula 2. CS30 DroprateThe suitable upper limit range is 1.00 or less, 0.70 or less, 0.50 or less, 0.45 or less, 0.40 or less, 0.35 or less, 0.32 or less, 0.30 or less, 0.28 or less, 0.25 or less, and particularly 0.20 or less. If CS30 Droprate Small, then CS30 2nd On the other hand, the lower limit is not particularly limited, but is 0.05 or more, 0.10 or more, and particularly 0.15 or more.
[0202] [Mathematical formula 2]
[0203]
[0204] [Example]
[0205] Hereinafter, the present invention will be described based on examples. It should be noted that the following examples are only for illustration purposes and the present invention is not limited in any way by the following examples.
[0206] (Example 1)
[0207] Tables 1 to 30 show the glass compositions and glass properties of the examples (samples No. 001 to 102, No. 104 to 285) and the comparative example (sample No. 103) of the present invention. It should be noted that "NA" in the table means not measured, and "R2O / Al2O3" means the molar ratio ([Li2O]+[Na2O]+[K2O]+) / [Al2O3].
[0208] [Table 1]
[0209]
[0210] [Table 2]
[0211]
[0212] [Table 3]
[0213]
[0214] [Table 4]
[0215]
[0216] [Table 5]
[0217]
[0218] [Table 6]
[0219]
[0220] [Table 7]
[0221]
[0222] [Table 8]
[0223]
[0224] [Table 9]
[0225]
[0226] [Table 10]
[0227]
[0228] [Table 11]
[0229]
[0230] [Table 12]
[0231]
[0232] [Table 13]
[0233]
[0234] [Table 14]
[0235]
[0236] [Table 15]
[0237]
[0238] [Table 16]
[0239]
[0240] [Table 17]
[0241]
[0242] [Table 18]
[0243]
[0244] [Table 19]
[0245]
[0246] [Table 20]
[0247]
[0248] [Table 21]
[0249]
[0250] [Table 22]
[0251]
[0252] [Table 23]
[0253]
[0254] [Table 24]
[0255]
[0256] [Table 25]
[0257]
[0258] [Table 26]
[0259]
[0260] [Table 27]
[0261]
[0262] [Table 28]
[0263]
[0264] [Table 29]
[0265]
[0266] [Table 30]
[0267]
[0268] Each sample in the table was prepared as follows. First, glass raw materials were prepared in such a way that the glass composition in the table was obtained, and melted at 1600°C for 21 hours using a platinum pot. Next, the obtained molten glass was flowed onto a carbon plate, formed into a flat plate shape, and then cooled at 3°C / min in the temperature range between the annealing point and the strain point to obtain a glass plate (glass plate for strengthening). The surface of the obtained glass plate was optically polished in such a way that the plate thickness became 1.5 mm, and then various properties were evaluated.
[0269] The density (ρ) is a value measured by the known Archimedean method.
[0270] The softening point (Ts) is a value measured by the method of ASTM C338.
[0271] Thermal expansion coefficient (α) at 30-380°C 30-380℃) is a value obtained by measuring the average thermal expansion coefficient using a dilatometer.
[0272] High temperature viscosity 10 2.5 dPa·s at temperature (10 2.5 dPa·s) is a value measured by a platinum ball pulling method.
[0273] The Young's modulus (E) is calculated by a method in accordance with JIS R1602-1995 "Test method for elastic modulus of fine ceramics".
[0274] Next, each unstrengthened glass plate (strengthening glass plate) was immersed in a KNO3 molten salt at 430°C for 4 hours to perform an ion exchange treatment, thereby obtaining a strengthened glass plate having a compressive stress layer on the surface. The glass surface was then cleaned, and then the compressive stress value (CS) of the outermost surface of the compressive stress layer was calculated from the number and interval of interference fringes observed using a surface stress meter FSM-6000 (manufactured by Orihara Seisakusho Co., Ltd.). K ) and stress depth (DOL K ). Here, DOL K This is the depth of the layer when ion exchange is performed using the above-mentioned KNO3 molten salt.
[0275] In addition, each unstrengthened glass plate (strengthening glass plate) was immersed in a molten salt of NaNO3 at 380°C for 1 hour to perform ion exchange treatment to obtain a strengthened glass plate. The glass surface was then cleaned and the compressive stress value (CS) of the outermost surface was calculated from the phase difference distribution curve observed using a scattered light photoelastic stress meter SLP-2000 (manufactured by Orihara Seisakusho Co., Ltd.). Na ), compressive stress value at a depth of 30 μm (CS30 Na ) and stress depth (DOC Na ), and internal tensile stress value (CTcv Na ). Here, DOC Na It is the depth of the compressive stress layer when ion exchange is performed using the above-mentioned NaNO3 molten salt, and is the depth at which the stress value becomes zero.
[0276] For the acid resistance test, a glass sample with a size of 50×10×1.0 mm was used as a test sample. After being thoroughly cleaned with a neutral detergent and pure water, it was immersed in a 5 mass % HCl aqueous solution heated to 80° C. for 24 hours, and the mass loss per unit surface area (mg / cm) before and after the immersion was calculated. 2 ), and thus make an evaluation.
[0277] For the alkali resistance test, a glass sample with a size of 50×10×1.0 mm was used as a test sample. After being thoroughly cleaned with a neutral detergent and pure water, it was immersed in a 5 mass % NaOH aqueous solution heated to 80°C for 6 hours, and the mass loss per unit surface area (mg / cm2) before and after immersion was calculated. 2 ), and thus make an evaluation.
[0278] The fracture toughness (K1c) was measured by the SEPB method in accordance with JIS R1607 "Test method for fracture toughness of fine ceramics". The fracture toughness value of each sample was obtained from the average value of three points.
[0279] As shown in Tables 1 to 30, for the tempered glass sheets of Samples Nos. 001 to 102 and 104 to 285, since the contents of [B2O3] + [MgO] + [CaO] and the molar ratio ([Li2O] + [Na2O] + [K2O]) / [Al2O3] are appropriate, the compressive stress value (CS) of the outermost surface of the compressive stress layer when ion exchanged with NaNO3 is Na ) is as large as 202MPa or more, and the compressive stress value (CS30 Na ) is as large as 41MPa or more. Therefore, it is considered that it is easy to make Figure 3 The stress curve with such an inflection point is less likely to be broken when dropped than Sample No. 103 which is a comparative example.
[0280] In addition, for the glass plate No. 071 (glass plate for strengthening), after being immersed in a NaNO3 molten salt at 380°C for 4.5 hours, it was immersed in a KNO3 molten salt at 430°C for 30 minutes. As a result, it was confirmed that the compressive stress value CS of the outermost surface of the compressive stress layer was further increased to 768 MPa, and the compressive stress value CS30 at a depth of 30 μm from the outermost surface was further increased to 148 MPa.
[0281] In addition, for the glass plate No. 106 (glass plate for strengthening), after being immersed in a NaNO3 molten salt at 380°C for 2 hours, it was immersed in a mixed molten salt of 92.5 mass% KNO3 and 7.5 mass% NaNO3 at 410°C for 24 minutes. As a result, it was confirmed that the compressive stress value CS of the outermost surface of the compressive stress layer was further increased to 873 MPa, and the compressive stress value CS30 at a depth of 30 μm from the outermost surface was further increased to 154 MPa.
[0282] In addition, for the glass plate No. 247 (glass plate for strengthening), after being immersed in a NaNO3 molten salt at 380°C for 77 minutes, it was immersed in a mixed molten salt of 92.5 mass% KNO3 and 7.5 mass% NaNO3 at 410°C for 25 minutes. As a result, it was confirmed that the compressive stress value CS of the outermost surface of the compressive stress layer was further increased to 878 MPa, and the compressive stress value CS30 at a depth of 30 μm from the outermost surface was further increased to 167 MPa.
[0283] (Example 2)
[0284] A 0.7 mm thick unreinforced glass plate (reinforced glass plate) having the same composition as sample No. 071 of Example 1 was immersed in a NaNO 3 molten salt at 380°C for 540 minutes and then immersed in a KNO 3 molten salt at 430°C for the time described in Table 12 to obtain a reinforced glass plate.
[0285] Furthermore, the stress curve of the obtained tempered glass plate was measured using a scattered light photoelastic stress meter SLP-2000 (manufactured by Orihara Corporation) and a surface stress meter FSM-6000 (manufactured by Orihara Corporation). Figure 4 is the overall image of the stress curves of Examples 2-1 to 2-3, Figure 5 Yes Figure 4 The stress curve shown is an enlarged view of the low compressive stress region. Figure 4 , Figure 5 Although the stress curve of one main surface of the strengthened glass plate is shown, the same stress curve is observed for the back surface.
[0286] Table 31 shows the strengthening conditions and glass properties of Examples 2-1 to 2-3. In the table, "SPP-4PB" means four-point bending strength after damage.
[0287] [Table 31]
[0288]
[0289] For each sample (Examples 2-1 to 2-3), after cleaning the glass surface, the compressive stress value (CS) of the outermost surface and the depth De of the bending point were calculated using a surface stress meter FSM-6000 (manufactured by Orihara Seisakusho Co., Ltd.). It should be noted that the value of the depth of the bending point (De) in the table represents the value of the diffusion depth DOL of K ions obtained by FSM-6000 (De=DOL). In the tempered glass plates such as Examples 2-1 to 2-3, that is, the tempered glass plates in which the Li ions in the glass were exchanged with the Na ions in the molten salt by the first ion exchange (without exchanging the K ions) and the Na ions in the glass were exchanged with the K ions in the molten salt by the second ion exchange, the depth De of the bending point e is substantially consistent with the diffusion depth DOL of the K ions.
[0290] In addition, the compressive stress values (CS30 and CS50) and stress depth (DOC) at depths of 30 μm and 50 μm, and the internal tensile stress value (CT) were calculated from the phase difference distribution curve observed using a scattered light photoelastic stress meter SLP-2000 (manufactured by Orihara Corporation).
[0291] The 4-point bending strength after damage is measured according to the following steps. First, the glass is damaged according to the following steps. A tempered glass plate that has been processed into a size of 50 mm × 50 mm and a thickness as shown in Table 31 is fixed vertically to a 1.5 mm thick SUS plate, and the end of a pendulum-shaped arm is made to collide with it through sandpaper with a grit number of P 180 to cause damage. The end of the arm is a φ5 mm iron cylinder, and the arm weight is 550 g. The height of the downward swing of the arm is set to 5 mm from the collision point. Next, the damaged sample is subjected to a 4-point bending test based on JIS R1601 (1995) to measure the strength.
[0292] From Table 31 and Figure 4 , Figure 5 It can be seen that in Examples 2-1 to 2-3, the compressive stress value (CS) of the outermost surface of the compressive stress layer is as large as 815 MPa or more, and the compressive stress value (CS30) at a depth of 30 μm from the outermost surface is as large as 148 MPa or more. In addition, since the 4-point bending strength after damage is as high as 199 MPa or more, it is believed that it is not easy to break when dropped.
[0293] (Example 3)
[0294] For an unreinforced glass plate (reinforced glass plate) with a thickness of 0.7 mm having the same composition as Sample No. 106 and No. 247 of Example 1, after being immersed in a NaNO3 molten salt at 380°C for the time recorded in Table 32, it was immersed in a KNO3 molten salt at 430°C for the time recorded in Table 32 to obtain a reinforced glass plate.
[0295] Furthermore, the same method as in Example 2 was used to measure the stress curve of the obtained tempered glass plate. Figure 6 is the overall image of the stress curves of Examples 3-1 and 3-2, Figure 7 Yes Figure 6 An enlarged view of the low compressive stress region in the stress curve is shown.
[0296] Table 32 shows the strengthening conditions and glass properties of Examples 3-1 and 3-2.
[0297] [Table 32]
[0298]
[0299] For each sample (Examples 3-1 and 3-2), the stress value and stress depth were measured by the same method as in Example 2, and then the four-point bending strength after damage was measured.
[0300] From Table 32 and Figure 6 , Figure 7 It can be seen that in Examples 3-1 and 3-2, the compressive stress value (CS) of the outermost surface of the compressive stress layer is as large as 892 MPa or more, and the compressive stress value (CS30) at a depth of 30 μm from the outermost surface is as large as 146 MPa or more. In addition, the 4-point bending strength after damage is as high as 199 MPa or more, so it is believed that it is not easy to break when falling.
[0301] (Example 4)
[0302] For an unreinforced glass plate (reinforced glass plate) with a thickness of 0.7 mm and the same composition as sample No. 277 in Example 1, after being immersed in a NaNO3 molten salt at 380°C for the time recorded in Table 33, it was immersed in a KNO3 molten salt at 430°C for the time recorded in Table 33 to obtain a reinforced glass plate.
[0303] Furthermore, the same method as in Example 2 was used to measure the stress curve of the obtained tempered glass plate. Figure 8 is the overall image of the stress curves of Examples 4-1 to 4-4, Fig. 9 Yes Figure 8 An enlarged view of the low compressive stress region in the stress curve is shown.
[0304] Table 33 shows the strengthening conditions and glass properties of Examples 4-1 to 4-4.
[0305] [Table 33]
[0306]
[0307] For each sample (Examples 4-1 to 4-4), the stress value and stress depth were measured by the same method as in Example 2, and then the 4-point bending strength after damage was measured.
[0308] From Table 33 and Figure 8 , Fig. 9 It can be seen that in Example 4-1, the compressive stress value (CS) of the outermost surface of the compressive stress layer is as high as 739 MPa, and the compressive stress value (CS30) at a depth of 30 μm from the outermost surface is as high as 113 MPa. In addition, the 4-point bending strength after damage is as high as 167 MPa, so it is believed that it is not easy to break when dropped.
[0309] (Example 5)
[0310] An unreinforced glass plate (reinforced glass plate) having the same composition as the sample described in Example 1 (sample No. described in Tables 34 to 41) and a thickness of 0.7 mm was immersed in the molten salt described in Tables 34 to 41 for the time described to obtain a reinforced glass plate subjected to two-stage ion exchange.
[0311] Tables 34 to 41 show the strengthening conditions and glass properties of Examples 5-1 to 5-86.
[0312] [Table 34]
[0313]
[0314] [Table 35]
[0315]
[0316] [Table 36]
[0317]
[0318] [Table 37]
[0319]
[0320] [Table 38]
[0321]
[0322] [Table 39]
[0323]
[0324] [Table 40]
[0325]
[0326] [Table 41]
[0327]
[0328] For each of the obtained samples (Examples 5-1 to 5-86), the compressive stress value (CS30 at a depth of 30 μm) of the tempered glass plate after the first ion exchange was measured using a scattered light photoelastic stress meter SLP-2000 (manufactured by Orihara Seisakusho Co., Ltd.). 1st ), the compressive stress value at a depth of 30 μm of the strengthened glass plate after the second ion exchange (CS30 2nd ), calculate the compressive stress reduction rate at a depth of 30 μm (CS30 Droprate ).
[0329] It can be seen from Tables 34 to 41 that the compressive stress reduction rates (CS30 Droprate ) is as low as 0.61 or less. It is considered easy to make Figure 3 Such a stress curve with a bending point is not easily damaged when falling.
[0330] (Example 6)
[0331] For samples No. 055, No. 072, No. 106, No. 116, and No. 247 of Example 1, the mutual diffusion coefficient D of Na ions was measured. Na The mutual diffusion coefficient D of K ions K .
[0332] First, a tempered glass having the same composition as the above samples was prepared, and ion exchange was performed with 100% NaNO3 at 380°C for the time t described in Table 42 to obtain a tempered glass plate. Then, the Na ion concentration distribution of the cut surface was measured by line scanning of EPMA. The EPMA measurement was performed using JXA-8100 manufactured by JEOL, with the acceleration voltage set to 15 kV, the current set to 500 nA, the measurement interval set to 0.82 μm, and the electron beam diameter set to 2 μm.
[0333] The obtained ion concentration distribution was approximated by curve using the analytical solution of Fick's diffusion equation. Specifically, the Na ion concentration C at the outermost surface (x = 0) was used. max and the Na ion concentration C at depth (x = +∞) min , the concentration distribution at the enhancement time t obtained by EPMA is normalized to fit the complementary error function erfc By inputting each value into the above mathematical formula 1, the value of D is derived using the least squares method as the mutual diffusion coefficient D Na It should be noted that the Na ion concentration C in the deep part (x = +∞) min The average value of the Na ion concentration at a depth of 300 μm to 400 μm was used. Fig.10It is a curve of the measured values of the Na ion concentration of the tempered glass plate obtained by ion exchange of sample No. 247 under the conditions described in Table 42, measured by EPMA, and the results obtained by approximating the measured values with the complementary error function.
[0334] The mutual diffusion coefficient D for K ions K In terms of the above mutual diffusion coefficient D Na In the calculation method of , the molten salt used was changed to 100% KNO3, and the measurement object of EPMA was changed to K ions, thereby deriving using the same method.
[0335] [Table 42]
[0336]
[0337] In addition, for unreinforced glass plates (reinforced glass plates) with a thickness of 0.7 mm having the same composition as Samples No. 055, No. 072, No. 106, No. 116, and No. 247 of Example 1, a first ion exchange was performed under the conditions described in Table 43, and then a second ion exchange was performed under the conditions described in the table, thereby obtaining reinforced glass.
[0338] [Table 43]
[0339]
[0340] For each of the obtained samples (Examples 6-1 to 6-5), the compressive stress value and the compressive stress depth value were measured by the same method as in Examples 2 to 5, and then the four-point bending strength after damage was measured.
[0341] It can be seen from Table 42 and Table 43 that for the glasses of Examples 6-1 to 6-5, the ratio of the mutual diffusion coefficients D K / D Na is 0.0008 or more, the compression stress reduction rate (CS30 Droprate ) is below 0.46, the compressive stress value (CS) of the outermost surface of the compressive stress layer after two stages of ion exchange is as large as 725MPa or more, and the compressive stress value (CS30) at a depth of 30μm from the outermost surface is as large as 125MPa or more. In addition, the 4-point bending strength after damage is as high as 176MPa or more, so it is considered that it is not easy to break when falling.
[0342] Industrial Applicability
[0343] The tempered glass plate of the present invention is suitable as a cover glass for a touch panel display of a mobile phone, a digital camera, a PDA (portable terminal), etc. In addition to these uses, the tempered glass plate of the present invention is also expected to be used in uses requiring high mechanical strength, such as window glass, a substrate for a magnetic disk, a substrate for a flat panel display, a substrate for a flexible display, a cover glass for a solar cell, a cover glass for a solid-state image sensor device (Japanese original: solid-state image sensor), and a cover glass for a vehicle.
[0344] Description of Reference Numerals
[0345] a The first peak
[0346] b Valley 1
[0347] c Peak 2
[0348] d Valley 2
[0349] e bending point
Claims
1. A tempered glass plate, characterized in that: It has a compressive stress layer on the surface, and contains, as a glass composition, in mol %, SiO2 50% to 80%, Al2O3 7% to 25%, B2O3 0% to 15%, Li2O 0% to 15%, Na2O 0% to 25%, K2O 0% to 10%, MgO 0% to 15%, CaO 0% to 10%, SrO 0% to 10%, BaO 0% to 10%, ZnO 0% to 10%, P2O5 0% to 15%, TiO2 0% to 10%, ZrO2 0% to 10%, SnO2 0% to 0.30%, [B2O3] + [MgO] + [CaO] is 0.1% to 30%, and ([Li2O] + [Na2O] + [K2O]) / [Al2O3] is 0.5 to 2.
0.
2. The tempered glass sheet according to claim 1, wherein: The Z value calculated by the following formula is 18.0 or more. Z=0.13×[SiO2]+2.36×[Al2O3]-0.14×[B2O3]+4.90×[Li2O]-5.53×[Na2O]-2.14×[MgO]-2.34×[CaO].
3. The tempered glass sheet according to claim 2, wherein: The Z value calculated by the following formula is 20.0 or more. Z=0.13×[SiO2]+2.36×[Al2O3]-0.14×[B2O3]+4.90×[Li2O]-5.53×[Na2O]-2.14×[MgO]-2.34×[CaO].
4. The tempered glass sheet according to claim 1 or 2, wherein: The molar ratio [Na2O] / [Li2O] is 1.0 or less.
5. The tempered glass sheet according to claim 1 or 2, wherein: The Y value calculated by the following formula is 5.0 or more, Y=3+0.21×[SiO2]+0.25×[Al2O3]-0.33×[B2O3]-0.55×[Li2O]+0. 45×[Na2O]-0.97×[MgO]-1.46×[CaO].
6. The tempered glass sheet according to claim 5, wherein: The Y value calculated by the following formula is 6.0 to 30, Y=3+0.21×[SiO2]+0.25×[Al2O3]-0.33×[B2O3]-0.55×[Li2O]+0. 45×[Na2O]-0.97×[MgO]-1.46×[CaO].
7. The tempered glass sheet according to claim 1 or 2, wherein: The X value calculated by the following formula is 300 or more. X=-1.49×[SiO2]+26.98×[Al2O3]-3.23×[B2O3]+48.56×[Li2O]-24.31×[Na2O]-0.28×[MgO]+2.74×[CaO].
8. The tempered glass sheet according to claim 1 or 2, wherein: The W value calculated by the following formula is 340 or more, W=0.07×[SiO2]+18.17×[Al2O3]-4.42×[B2O3]+41.43×[Li2O]- 29.30×[Na2O]+1.43×[MgO]-10.43×[CaO].
9. The tempered glass plate according to claim 1 or 2, wherein: [Al2O3]+[Li2O]+[Na2O]+[K2O] is more than 10.5%.
10. The tempered glass sheet according to claim 1 or 2, wherein: The molar ratio [Li2O] / [Al2O3] is greater than 0.
1.
11. The tempered glass sheet according to claim 1 or 2, wherein: The U value calculated by the following formula is 7000 or more. U=87.39×[SiO2]+180.12×[Al2O3]+93.63×[B2O3]+113.78× ([MgO]+[CaO]+[BaO]+[SrO])-46.2×[Li2O]-71.1×[Na2O]-58.6×[K2O]-40.0×[P2O5].
12. The tempered glass sheet according to claim 1 or 2, wherein: The Q value calculated by the following formula is -30 or more. Q=[SiO2]+1.2×[P2O5]-3×[Al2O3]-[B2O3]-2×[Li2O]-1.5×[Na2O]-[K2O].
13. The tempered glass sheet according to claim 1 or 2, wherein: The glass composition contains Cl, and the content of Cl is 0.02 mol% or more.
14. The tempered glass sheet according to claim 1 or 2, wherein: The glass composition contains MoO3, and the content of MoO3 is 0.0001 mol% or more.
15. The tempered glass sheet according to claim 1 or 2, wherein: The softening point Ts is 920°C or less.
16. The tempered glass sheet according to claim 1 or 2, wherein: The compressive stress value CS of the outermost surface of the compressive stress layer is 200MPa to 1400MPa. The stress depth DOC of the compressive stress layer is 3 μm to 200 μm.
17. The tempered glass sheet according to claim 1 or 2, wherein: The stress depth DOC of the compressive stress layer is 50 μm to 200 μm. The compressive stress value CS30 at a depth of 30 μm from the outermost surface is 35 MPa to 400 MPa.
18. The tempered glass sheet according to claim 1 or 2, wherein: High temperature viscosity 10 2 The temperature at .5dPa·s is below 1680°C.
19. The tempered glass sheet according to claim 1 or 2, wherein: An overflow confluence surface is provided inside.
20. The tempered glass sheet according to claim 1 or 2, wherein: The stress curve in the thickness direction has an inflection point.
21. A tempered glass plate, characterized in that: The glass composition includes, by mol%, SiO2 50% to 80%, Al2O3 7% to 25%, B2O3 1% to 15%, Li2O 0% to 15%, Na2O 0% to 25%, K2O 0% to 10%, MgO 0% to 15%, CaO 0% to 10%, BaO 0% to 10%, SrO 0% to 10%, ZnO 0% to 10%, P2O5 0% to 4%, TiO2 0.00 1% to 0.1%, ZrO2 0% to 10%, Fe2O3 0.00 1% to 0.1%, SnO2 0.00 1%~0.30%, [B2O3]+[MgO]+[CaO] is 0.1%~30%, and ([Li2O]+[Na2O]+[K2O]) / [Al2O3] is 0.5~2.
0.
22. A method for manufacturing a tempered glass plate, characterized in that: The following processes are available: The preparation step is to prepare a tempered glass plate, wherein the tempered glass plate contains, as a glass composition, SiO2 50% to 80%, Al2O3 7% to 25%, B2O3 0% to 15%, Li2O 0% to 15%, Na2O 0% to 25%, K2O 0% to 10%, MgO 0% to 15%, CaO 0% to 10%, BaO 0% to 10%, SrO 0% to 10%, ZnO 0% to 10%, P2O5 0% to 15%, TiO2 0% to 10%, ZrO2 0% to 10%, SnO2 0% to 0.30%, [B2O3] + [MgO] + [CaO] is 0.1% to 30%, and ([Li2O] + [Na2O] + [K2O]) / [Al2O3] is 0.5 to 2.0; as well as In the ion exchange step, the tempered glass plate is subjected to multiple ion exchange treatments to obtain a tempered glass plate having a compressive stress layer on the surface.
23. A tempered glass plate, characterized in that: The glass composition contains, in mol%, SiO2 50% to 80%, A12O3 7% to 25%, B2O3 0% to 15%, Li2O 0% to 15%, Na2O 0% to 25%, K2O 0% to 10%, MgO 0% to 15%, CaO 0% to 10%, BaO 0% to 10%, SrO 0% to 10%, ZnO 0% to 10%, P2O5 0% to 15%, TiO2 0% to 10%, ZrO2 0% to 10%, SnO2 0% to 0.30%, [B2O3] + [MgO] + [CaO] is 0.1% to 30%, and ([Li2O] + [Na2O] + [K2O]) / [Al2O3] is 0.5 to 2.
0.
24. The tempered glass plate according to claim 23, wherein: The Na ion mutual diffusion coefficient D at 380℃ Na 1×10 -14 m 2 sec -1 ~1×10 -11 m 2 sec -1 , K ion mutual diffusion coefficient D at 380℃ K 1×10 -17 m 2 sec -1 ~1×10 -14 m 2 sec -1 , D K / D Na is 0.000 1 or more.
Citation Information
Patent Citations
Glass member
JP2006083045A
Cited By
Ultrathin glass, reinforced impact-resistant ultrathin glass and preparation method and application thereof
CN120271224A
Ultra-thin glass and strengthened impact-resistant ultra-thin glass, and methods of making and use thereof
CN120271224B
High-modulus glass, protective film, cover plate layer, display module, and electronic device
WO2026144573A1