Steel sheet, member, and method for manufacturing same

The steel plate's optimized composition and manufacturing process address the challenges of press formability and energy absorption, achieving high strength and formability suitable for automotive impact energy absorption.

WO2024202803A1PCT designated stage expired Publication Date: 2024-10-03JFE STEEL CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/006906
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-02-27
Publication Date
2024-10-03

Smart Images

  • Figure JP2024006906_03102024_PF_FP_ABST
    Figure JP2024006906_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a steel sheet, a member, and methods for manufacturing same, the steel sheet having a tensile strength of 1180 MPa or more and less than 1470 MPa and having a high yield stress, a high yield ratio, excellent press formability (bendability and ductility of the steel sheet), and an excellent energy absorption characteristic. The base steel sheet has a predetermined component composition and has a surface soft layer of 20 μm or more on the surface layer of the base steel sheet. In the steel structure at a position of 1 / 4 of the plate thickness of the base steel sheet, ferrite, retained austenite, fresh martensite, bainitic ferrite, and tempered martensite are set within a predetermined range where LF - MA / LF : 0.70 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Steel plates, components, and their manufacturing methods

[0001] The present invention relates to a steel plate, a member made from the steel plate, and a method for manufacturing the same.

[0002] From the perspective of protecting the global environment, improving the fuel efficiency of automobiles has become an important issue. Therefore, there has been a growing movement to reduce the weight of automobile bodies by increasing the strength and thinning of steel sheets, which are the raw materials for automobile parts.

[0003] In addition, social demands for improved automobile crashworthiness are increasing, and therefore there is a need for the development of steel sheets that not only have high strength but also excellent impact resistance in the event of a collision while the automobile is in motion (hereinafter simply referred to as impact resistance).

[0004] As an example of a steel sheet that can be used as a material for such automotive parts, Patent Document 1 discloses a high-strength hot-dip galvanized steel sheet having a component composition containing, by mass%, 0.05 to 0.3% C, 0.01 to 2.5% Si, 0.5 to 3.5% Mn, 0.003 to 0.100% P, 0.02% or less S, 0.010 to 1.5% Al, 0.007% or less N, with the balance being Fe and unavoidable impurities, and having a microstructure containing, by area ratio, 20 to 87% ferrite, 3 to 10% martensite and retained austenite in total, and 10 to 60% tempered martensite, with a high TS-El balance, excellent stretch flangeability, and low YR and excellent workability.

[0005] Patent Document 2 also describes a high-strength hot-dip galvanized steel sheet having a thickness of 0.6 to 5.0 mm and a plating layer on the surface of the steel sheet, the steel sheet structure containing 40 to 90% by volume of a ferrite phase and 3 to 25% by volume of a retained austenite phase, the retained austenite phase having a solute carbon content of 0.70 to 1.00%, an average particle size of 2.0 μm or less, an average distance between particles of 0.1 to 5.0 μm, a thickness of a decarburized layer in the surface layer of the steel sheet of 0.01 to 10.0 μm, an average particle size of oxides contained in the surface layer of the steel sheet of 30 to 120 nm, and an average density of 1.0 × 10 12 pieces / m 2The above also discloses a high-strength hot-dip galvanized steel sheet that has excellent mechanical cutting properties, while ensuring high strength of a maximum tensile strength of 900 MPa or more, and is characterized by having an average work-hardening coefficient (n value) of 0.080 or more at the time of plastic deformation of 3 to 7%.

[0006] Furthermore, Patent Document 3 discloses a high-strength hot-dip galvanized steel sheet excellent in delayed fracture resistance, characterized in that the steel sheet has, by volume fraction, 40 to 90% of a ferrite phase and 5% or less of a retained austenite phase, the proportion of unrecrystallized ferrite in the entire ferrite phase being 50% or less, the grain size ratio, which is the value obtained by dividing the average grain size of crystal grains of the ferrite phase in the rolling direction by the average grain size in the sheet width direction, is 0.75 to 1.33, the length ratio, which is the value obtained by dividing the average length of hard structures dispersed in an island shape in the rolling direction by the average length in the sheet width direction, is 0.75 to 1.33, and the average aspect ratio of inclusions is 5.0 or less.

[0007] Patent No. 5256689 Patent No. 5354135 Patent No. 5352793

[0008] In recent years, the practical application of steel sheets having a tensile strength (hereinafter also referred to as TS) of 780 MPa or more has been increasing for impact energy absorbing members of automobiles, such as front side members and rear side members.

[0009] That is, improving the yield stress (hereinafter also referred to as YS) is effective in increasing the energy absorption during impact (hereinafter also referred to as impact absorption energy). However, increasing the TS and YS of a steel sheet generally reduces press formability, particularly properties such as ductility, hole expandability, and bendability. Therefore, when applying a steel sheet with such increased TS and YS to the above-mentioned automotive impact energy absorbing components, press forming becomes difficult, and variations during forming result in a decrease in yield. In particular, a decrease in press formability at the end of the steel sheet leads to the occurrence of end cracks in the actual component.

[0010] Patent Document 1 discloses a high-strength hot-dip galvanized steel sheet that has improved ductility, which is the press formability of the interior of the steel sheet, and stretch flangeability, which is the press formability of the steel sheet end portion. However, it cannot be said that the bendability and energy absorption characteristics are sufficient.

[0011] Patent Document 2 discloses a high-strength hot-dip galvanized steel sheet in which ductility is improved by generating retained austenite inside the steel sheet and mechanical cutting properties are improved by forming a decarburized layer on the surface layer of the steel sheet. However, it cannot be said that the bendability and energy absorption properties are sufficient.

[0012] Patent Document 3 discloses a high-strength hot-dip galvanized steel sheet in which the main structure inside the steel sheet is soft ferrite and the amount of unrecrystallized ferrite is limited to a small amount, thereby improving ductility, and the delayed fracture resistance and anisotropy thereof are improved by forming a decarburized layer in the surface layer of the steel sheet. However, it cannot be said that the bendability and energy absorption characteristics are sufficient.

[0013] From the above, it cannot be said that the steel sheets disclosed in Patent Documents 1 to 3 have a TS of 1180 MPa or more, a high YS, a high yield ratio YR, excellent press formability (bendability and ductility of the steel sheet), and excellent energy absorption characteristics.

[0014] The present invention has been made in consideration of the above problems, and aims to provide a steel sheet having a tensile strength TS of 1180 MPa or more and less than 1470 MPa, a high yield stress YS, a high yield ratio YR, excellent press formability (bendability and ductility of the steel sheet), and excellent energy absorption characteristics, together with an advantageous manufacturing method thereof. Another aim of the present invention is to provide a member made from the above steel sheet, and a manufacturing method thereof.

[0015] The steel sheet referred to here also includes a galvanized steel sheet, and the galvanized steel sheet is a hot-dip galvanized steel sheet (hereinafter also referred to as GI), a galvannealed hot-dip galvanized steel sheet (hereinafter also referred to as GA), or an electro-galvanized steel sheet (hereinafter also referred to as EG).

[0016] Here, the tensile strength TS is measured by a tensile test in accordance with JIS Z 2241 (2011).

[0017] Furthermore, having a high yield stress YS, a high yield ratio YR, excellent press formability (bendability and ductility of the steel sheet), and excellent energy absorption characteristics means satisfying the following.

[0018] A high yield stress YS means that the YS measured in a tensile test in accordance with JIS Z 2241 (2011) satisfies the following formula (A) or (B) depending on the TS measured in the tensile test: (A) 750 MPa ≦ YS when 1180 MPa ≦ TS < 1320 MPa; (B) 850 MPa ≦ YS when 1320 MPa ≦ TS.

[0019] Furthermore, a high yield ratio YR means that the YR calculated based on the yield stress YS and tensile strength TS measured in a tensile test in accordance with JIS Z 2241 (2011) is 0.70 or more.

[0020] Furthermore, excellent bendability means that the bending angle (α) at ​​maximum load measured in a bending test in accordance with the VDA standard (VDA238-100) specified by the German Association of the Automotive Industry is 80° or more.

[0021] Furthermore, excellent ductility (excellent internal stretch formability of the steel sheet) means that the total elongation (El) measured in a tensile test in accordance with JIS Z 2241 (2011) satisfies the following formula (A) or (B) depending on the TS measured in the tensile test: (A) 11.0%≦El when 1180 MPa≦TS<1320 MPa; (B) 9.0%≦El when 1320 MPa≦TS.

[0022] Furthermore, excellent energy absorption characteristics means that, in addition to a high YS, the integral value AE of the load-stroke curve at the maximum load measured in a bending test in accordance with the VDA standard (VDA238-100) specified by the German Association of the Automotive Industry is 70,000 N mm or more.

[0023] The present inventors have conducted extensive research to achieve the above object. As a result, it has been found that the composition of the base steel sheet of the steel sheet can be properly adjusted and the total area ratio of the structures other than ferrite is S. A / 2 or less (S AWhen a region where the soft surface layer is a region where the area ratio is less than 20 μm in the thickness direction from the surface of the base steel sheet, the soft surface layer has a thickness of 20 μm or more from the surface of the base steel sheet in the thickness direction, and the structure at the 1 / 4 position of the thickness of the base steel sheet has an area ratio of ferrite: less than 20.0% (including 0.0%), a volume ratio of retained austenite: 3.0% or more and 15.0% or less, an area ratio of fresh martensite: 10.0% or less (including 0.0%), and a total area ratio of bainitic ferrite and tempered martensite (excluding retained austenite): 45.0% or more and 90.0% or less, and the grain boundary length L F―MA and the grain boundary length L of ferrite F Regarding L F―MA / L F The inventors have found that this makes it possible to obtain a steel sheet having a TS of 1180 MPa or more but less than 1470 MPa, a high YS, a high YR, excellent press formability (bendability and ductility of the steel sheet), and excellent energy absorption properties. The present invention has been completed based on the above findings and further investigations.

[0024] That is, the gist and configuration of the present invention are as follows. [1] A steel plate having a base steel plate, the base steel plate having a chemical composition containing, in mass%, C: 0.050% or more and 0.400% or less, Si: 0.20% or more and 3.00% or less, Mn: 1.00% or more and less than 3.50%, P: 0.001% or more and 0.100% or less, S: 0.0001% or more and 0.0200% or less, Al: 0.010% or more and 2.000% or less, and N: 0.0100% or less, with the balance being Fe and unavoidable impurities; and a structure at a 1 / 4 position of the plate thickness of the base steel plate having an area ratio of ferrite: less than 20.0% (including 0.0%), an area ratio of retained austenite: 3.0% or more and 15.0% or less, and an area ratio of fresh martensite: 10.0% or less (including 0.0%), The total area ratio of bainitic ferrite and tempered martensite is 45.0% or more and 90.0% or less, and the grain boundary length L of the ferrite grain boundary in contact with fresh martensite and / or retained austenite is F―MA and the grain boundary length L of ferrite F Regarding L F―MA / L F: 0.70 or less, and further comprising a surface soft layer formed to a thickness of 20 μm or more from the surface of the base steel sheet in the sheet thickness direction, wherein the total area ratio of structures other than ferrite in the steel structure is ½ or less at a position ¼ of the sheet thickness, and wherein the tensile strength is 1180 MPa or more and less than 1470 MPa. [2] The composition further includes, in mass%, Nb: 0.200% or less, Ti: 0.200% or less, V: 0.200% or less, B: 0.0100% or less, Cr: 1.000% or less, Ni: 1.000% or less, Mo: 1.000% or less, Sb: 0.200% or less, Sn: 0.200% or less, Cu: 1.000% or less, Ta: 0.100% or less, W: 0.500% or less, Mg: 0.0200% or less, Zn: 0.0200% or less, Co: 0.0200% or less, Zr: 0.1000% or less, Ca: 0.0200% or less, Se: 0.0200% or less, The steel sheet according to [1] above, containing at least one selected from Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0500% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, and REM: 0.0200% or less. [3] The steel sheet according to [1] or [2] above, wherein one or both sides of the base steel sheet are provided with a zinc-plated layer. [4] A member made using the steel sheet according to any one of [1] to [3] above.[5] A method of manufacturing a hot-rolled steel sheet by hot-rolling a steel slab having the chemical composition according to [1] or [2] above, comprising: a hot rolling process, in which a steel slab having the chemical composition according to [1] or [2] above is hot-rolled to form a hot-rolled steel sheet; a pickling process, in which the hot-rolled steel sheet is pickled; an annealing process, in which the steel sheet after the pickling process is heated and annealed under conditions of an annealing temperature of 720°C to 860°C, a holding time of 20 seconds or more, and an atmosphere with a dew point of -10°C or higher; a rapid heating process, in which the steel sheet is rapidly heated from the annealing temperature to a temperature of annealing temperature + 10°C or higher at a heating rate of 10°C / second or higher; a cooling process, in which the steel sheet after the rapid heating process is cooled to a cooling stop temperature of 100°C to 300°C; and a reheating and holding process, in which the steel sheet after the cooling process is heated to a tempering temperature range of 460°C or lower and held in the temperature range for a tempering time of 10 seconds to 2000 seconds, A method for producing a steel sheet, comprising a cold rolling step of cold rolling the steel sheet after the pickling step and before the annealing step at a rolling reduction of 20% or more and 80% or less to obtain a cold-rolled steel sheet. [6] The method for producing a steel sheet according to [5] above, wherein the threading speed LS (m / min) of the steel sheet in the annealing step satisfies the following formula (1): 3.0 / (t×W×4.716×10. ―4 )<LS<390.0 / (t×W×4.716×10 ―4 ) Formula (1) Wherein, t: sheet thickness (mm) after the pickling process and before the annealing process, and W: sheet width (mm) after the pickling process and before the annealing process. [7] The method for producing a steel sheet according to [5] or [6] above, comprising a hot-dip galvanizing step of immersing a steel sheet in a hot-dip galvanizing bath during the cooling step, after the cooling step and before the reheating and holding step, or after the reheating and holding step, to form a zinc-plated layer on the steel sheet, or further comprising an alloying treatment step of subjecting the steel sheet on which the zinc-plated layer has been formed to an alloying treatment. [8] The method for producing a steel sheet according to [5] or [6] above, comprising an electrogalvanizing step of immersing a steel sheet in an electrogalvanizing bath after the reheating and holding step, to form a zinc-plated layer on the steel sheet. [9] A method for producing a member, comprising a step of subjecting the steel sheet according to any of [1] to [3] above to at least one of forming and joining to form a member.

[0025] According to the present invention, a steel sheet can be obtained which has a tensile strength TS of 1180 MPa or more but less than 1470 MPa, a high yield stress YS, a high yield ratio YR, excellent press formability (bendability and ductility of the steel sheet), and excellent energy absorption properties. Furthermore, a member made from the steel sheet of the present invention has high strength, a high yield stress YS, a high yield ratio YR, excellent press formability (bendability and ductility of the steel sheet), and excellent energy absorption properties, and can be extremely advantageously used in automobile impact energy absorption members, etc.

[0026] 1 shows examples of SEM structural images used for structural identification, where (a) is a structural image of Comparative Example No. 19, and (b) is a structural image of Invention Example No. 1.

[0027] The present invention will be described based on the following embodiments.

[0028] [1. Steel Plate] The steel plate of the present invention is a steel plate having a base steel plate, the base steel plate containing, in mass%, C: 0.050% or more and 0.400% or less, Si: 0.20% or more and 3.00% or less, Mn: 1.00% or more and less than 3.50%, P: 0.001% or more and 0.100% or less, S: 0.0001% or more and 0.0200% or less, Al: 0.010% or more and 2.000% or less, and N: 0.0100% or less, with the balance being Fe and unavoidable impurities, and As for the structure, the area ratio of ferrite is less than 20.0% (including 0.0%), the area ratio of retained austenite is 3.0% or more and 15.0% or less, the area ratio of fresh martensite is 10.0% or less (including 0.0%), the total area ratio of bainitic ferrite and tempered martensite is 45.0% or more and 90.0% or less, and the grain boundary length L F―MA and the grain boundary length L of ferrite F Regarding L F―MA / L FThe steel sheet of the present invention has a steel structure satisfying a σ-σ ratio of 0.70 or less, and further has a soft surface layer formed to a thickness of 20 μm or more from the surface of the base steel sheet in the sheet thickness direction, where the total area ratio of structures other than ferrite in the steel structure is ½ or less at the ¼ position in the sheet thickness, and has a tensile strength of 1180 MPa or more and less than 1470 MPa. The steel sheet of the present invention has a tensile strength TS (hereinafter, tensile strength TS may also be simply referred to as TS) of 1180 MPa or more and less than 1470 MPa, a high yield stress YS (hereinafter, yield stress YS may also be simply referred to as YS), a high yield ratio YR (hereinafter, yield ratio YR may also be simply referred to as YR), excellent press formability (bendability and ductility of the steel sheet), and excellent energy absorption characteristics. The steel sheet may have a zinc-plated layer as the outermost layer on one or both sides of the steel sheet. The steel sheet having a zinc-plated layer may be a zinc-plated steel sheet. More specifically, a steel sheet having a hot-dip galvanized layer among zinc-coated layers may be referred to as a hot-dip galvanized steel sheet. A steel sheet having a galvannealed hot-dip galvanized layer among zinc-coated layers may be referred to as a galvannealed hot-dip galvanized steel sheet. A steel sheet having an electrogalvanized layer among zinc-coated layers may be referred to as an electrogalvanized steel sheet.

[0029] First, the chemical composition of the base steel sheet of the steel sheet according to one embodiment of the present invention will be described. Note that the units for the chemical compositions are all "mass %", but hereinafter, unless otherwise specified, they will be simply expressed as "%".

[0030] C: 0.050% or more and 0.400% or less. C is an effective element for generating appropriate amounts of fresh martensite, tempered martensite, bainitic ferrite, and retained austenite to ensure a TS of 1180 MPa or more and less than 1470 MPa and a high YS. Here, if the C content is less than 0.050%, the area fraction of ferrite increases, making it difficult to achieve a TS of 1180 MPa or more. This also results in a decrease in YS. On the other hand, if the C content exceeds 0.400%, the area fraction of fresh martensite increases excessively, making it difficult to achieve a TS of less than 1470 MPa. Furthermore, the increase in fresh martensite may introduce mobile dislocations into ferrite and bainitic ferrite, resulting in a decrease in YR. Furthermore, fresh martensite may serve as a starting point for void formation during VDA bending tests, potentially preventing the desired bendability of the steel sheet. Therefore, the C content is set to 0.050% or more and 0.400% or less. The C content is preferably 0.100% or more, and 0.300% or less.

[0031] Si: 0.20% or more and 3.00% or less Si suppresses the formation of carbides during cooling after annealing and promotes the formation of retained austenite. That is, Si is an element that affects the area fraction of retained austenite. Here, if the Si content is less than 0.20%, the area fraction of retained austenite decreases, and ductility decreases. On the other hand, if the Si content exceeds 3.00%, the YS may decrease due to an excessive increase in the area fraction of ferrite. Furthermore, the YR decreases. Therefore, the Si content is set to 0.20% or more and 3.00% or less. The Si content is preferably 2.00% or less. Furthermore, the Si content is preferably 0.50% or more.

[0032] Mn: 1.00% or more, less than 3.50% Mn is an element that adjusts the area ratio of bainitic ferrite, tempered martensite, etc. Here, if the Mn content is less than 1.00%, the area ratio of ferrite increases excessively, making it difficult to achieve a TS of 1180 MPa or more. It also leads to a decrease in YS. On the other hand, if the Mn content is 3.50% or more, the martensitic transformation start temperature Ms (hereinafter also referred to simply as the Ms point or Ms) decreases, and the amount of martensite formed during the cooling process decreases. As a result, the amount of martensite formed during final cooling increases, and the martensite formed at that time is not sufficiently tempered, resulting in an increase in the area ratio of hard fresh martensite. The increase in fresh martensite may introduce mobile dislocations into ferrite and bainitic ferrite, resulting in a decrease in YS. Furthermore, the YR decreases. Furthermore, fresh martensite serves as the starting point for void formation during the VDA bending test, which may prevent the desired bendability of the steel sheet from being achieved. Therefore, the Mn content is set to 1.00% or more and less than 3.50%, preferably 2.00% or more, and preferably 3.00% or less.

[0033] P: 0.001% or more and 0.100% or less P is an element that has a solid solution strengthening effect and increases the TS and YS of steel sheets. To achieve this effect, the P content is set to 0.001% or more. On the other hand, if the P content exceeds 0.100%, P segregates at prior austenite grain boundaries, embrittling the grain boundaries. As a result, the amount of voids generated during a VDA bending test increases, and there is a risk that the desired bendability cannot be achieved. Therefore, the P content is set to 0.001% or more and 0.100% or less. The P content is preferably 0.030% or less.

[0034] S: 0.0001% or more and 0.0200% or less S exists as sulfides in steel. In particular, if the S content exceeds 0.0200%, the amount of voids generated during the VDA bending test increases, and the desired bendability may not be achieved. Therefore, the S content is set to 0.0200% or less. The S content is preferably 0.0080% or less, and more preferably 0.0040% or less. Furthermore, due to constraints in production technology, the S content is set to 0.0001% or more, and preferably 0.0003% or more.

[0035] Al: 0.010% or more and 2.000% or less Al suppresses the formation of carbides during cooling after annealing and promotes the formation of retained austenite. That is, Al is an element that affects the volume fraction of retained austenite. To achieve this effect, the Al content is set to 0.010% or more. On the other hand, if the Al content exceeds 2.000%, the area fraction of ferrite increases excessively, making it difficult to achieve a TS of 1180 MPa or more. This also leads to a decrease in YS. Therefore, the Al content is set to 0.010% or more and 2.000% or less. The Al content is preferably 0.015% or more. The Al content is preferably 1.000% or less, more preferably 0.100% or less.

[0036] N: 0.0100% or less N exists as nitrides in steel. In particular, if the N content exceeds 0.0100%, the amount of voids generated during the VDA bending test increases, and the desired bendability may not be achieved. Therefore, the N content is set to 0.0100% or less. The N content is preferably 0.0050% or less. Although there is no particular lower limit for the N content, due to constraints in production technology, the N content is preferably 0.0005% or more, and more preferably 0.0010% or more.

[0037] The basic chemical composition of the base steel sheet of the steel sheet according to one embodiment of the present invention has been described above, but the base steel sheet of the steel sheet according to one embodiment of the present invention has a chemical composition containing the basic chemical components with the balance other than the basic chemical components including Fe (iron) and unavoidable impurities. Here, it is preferable that the base steel sheet of the steel sheet according to one embodiment of the present invention has a chemical composition containing the basic chemical components with the balance consisting of Fe and unavoidable impurities.

[0038] In addition to the basic components, the base steel sheet of a steel sheet according to one embodiment of the present invention may contain at least one selected from the optional components shown below. Note that the effects of the present invention can be obtained so long as the optional components shown below are contained in amounts up to the upper limit amounts shown below, so no lower limit is particularly set. Note that when the optional elements listed below are contained in amounts less than the preferred lower limit values ​​described below, the elements are considered to be included as inevitable impurities.

[0039] Nb: 0.200% or less, Ti: 0.200% or less, V: 0.200% or less, B: 0.0100% or less, Cr: 1.000% or less, Ni: 1.000% or less, Mo: 1.000% or less, Sb: 0. 200% or less, Sn: 0.200% or less, Cu: 1.000% or less, Ta: 0.100% or less, W: 0.500% or less, Mg: 0.0200% or less, Zn: 0.0200% or less, Co: 0.0200 %, Zr: 0.1000% or less, Ca: 0.0200% or less, Se: 0.0200% or less, Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0500% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, and at least one selected from REM: 0.0200% or less

[0040] Nb: 0.200% or less Nb forms fine carbides, nitrides, or carbonitrides during hot rolling or annealing, thereby increasing TS and YS. To achieve this effect, the Nb content is preferably 0.001% or more. The Nb content is more preferably 0.005% or more. On the other hand, if the Nb content exceeds 0.200%, a large amount of coarse precipitates and inclusions may be generated. In such cases, the amount of voids generated during the VDA bending test may increase, and the desired bendability may not be achieved. Therefore, when Nb is contained, the Nb content is preferably 0.200% or less. The Nb content is more preferably 0.060% or less.

[0041] Ti: 0.200% or less Like Nb, Ti increases TS and YS by forming fine carbides, nitrides, or carbonitrides during hot rolling or annealing. To achieve this effect, the Ti content is preferably 0.001% or more. The Ti content is more preferably 0.005% or more. On the other hand, if the Ti content exceeds 0.200%, a large amount of coarse precipitates or inclusions may be generated. In such cases, the amount of voids generated during the VDA bending test may increase, and the desired bendability may not be achieved. Therefore, when Ti is contained, the Ti content is preferably 0.200% or less. The Ti content is more preferably 0.060% or less.

[0042] V: 0.200% or less Like Nb and Ti, V forms fine carbides, nitrides, or carbonitrides during hot rolling and annealing, thereby increasing TS and YS. To achieve this effect, the V content is preferably 0.001% or more. The V content is more preferably 0.005% or more. The V content is further preferably 0.010% or more, and even more preferably 0.030% or more. On the other hand, if the V content exceeds 0.200%, a large amount of coarse precipitates and inclusions may be formed. In such cases, the amount of voids formed during the VDA bending test may increase, making it difficult to achieve the desired bendability. Therefore, when V is contained, the V content is preferably 0.200% or less. The V content is more preferably 0.060% or less.

[0043] B: 0.0100% or less B is an element that segregates at austenite grain boundaries to improve hardenability. Furthermore, B is an element that suppresses the formation and grain growth of ferrite during cooling after annealing. To achieve this effect, the B content is preferably 0.0001% or more. The B content is more preferably 0.0002% or more. The B content is further preferably 0.0005% or more, and even more preferably 0.0007% or more. On the other hand, if the B content exceeds 0.0100%, cracks may occur inside the steel sheet during hot rolling. Furthermore, the amount of voids generated during a VDA bending test may increase, making it difficult to achieve the desired bendability. Therefore, when B is contained, the B content is preferably 0.0100% or less. The B content is more preferably 0.0050% or less.

[0044] Cr: 1.000% or less. Cr is an element that improves hardenability, so the addition of Cr produces a large amount of tempered martensite, ensuring a TS of 1180 MPa or more and a high YS. To achieve this effect, the Cr content is preferably 0.0005% or more. The Cr content is more preferably 0.010% or more. The Cr content is even more preferably 0.030% or more, and even more preferably 0.050% or more. On the other hand, if the Cr content exceeds 1.000%, the area fraction of hard fresh martensite increases excessively, which may introduce mobile dislocations into ferrite and bainitic ferrite, resulting in a decrease in YS. Furthermore, fresh martensite may serve as a starting point for void formation during a VDA bending test, potentially preventing the desired bendability of the steel sheet. Therefore, when Cr is added, the Cr content is preferably 1.000% or less. The Cr content is more preferably 0.800% or less, further preferably 0.700% or less, and further more preferably 0.200% or less.

[0045] Ni: 1.000% or less. Ni is an element that improves hardenability, so the addition of Ni produces a large amount of tempered martensite, ensuring a TS of 1180 MPa or more and a high YS. To achieve this effect, the Ni content is preferably 0.005% or more. The Ni content is more preferably 0.020% or more. The Ni content is even more preferably 0.040% or more, and even more preferably 0.060% or more. On the other hand, if the Ni content exceeds 1.000%, the area fraction of fresh martensite increases excessively, which may introduce mobile dislocations into ferrite and bainitic ferrite, resulting in a decrease in YS. Furthermore, fresh martensite may serve as a starting point for void formation during a VDA bending test, potentially preventing the desired bendability of the steel sheet. Therefore, when Ni is contained, the Ni content is preferably 1.000% or less. The Ni content is more preferably 0.800% or less. The Ni content is more preferably 0.600% or less, and even more preferably 0.400% or less.

[0046] Mo: 1.000% or less Mo is an element that improves hardenability, and the addition of Mo results in the formation of a large amount of tempered martensite, ensuring a TS of 1180 MPa or more and a high YS. To achieve this effect, the Mo content is preferably 0.010% or more. The Mo content is more preferably 0.030% or more. On the other hand, if the Mo content exceeds 1.000%, the area fraction of fresh martensite increases excessively, which may introduce mobile dislocations into ferrite and bainitic ferrite, resulting in a decrease in YS. Furthermore, fresh martensite may serve as a starting point for void generation during a VDA bending test, potentially preventing the desired bendability of the steel sheet. Therefore, when Mo is added, the Mo content is preferably 1.000% or less. The Mo content is more preferably 0.500% or less, even more preferably 0.450% or less, and even more preferably 0.400% or less. The Mo content is more preferably 0.350% or less, even more preferably 0.300% or less, and more preferably 0.100% or less.

[0047] Sb: 0.200% or less Sb is an element that suppresses the diffusion of C near the steel sheet surface during annealing and is effective in controlling the formation of a soft layer near the steel sheet surface. If the soft layer increases excessively near the steel sheet surface, it becomes difficult to achieve a TS of 1180 MPa or more. It also leads to a decrease in YS. Therefore, the Sb content is preferably 0.002% or more. The Sb content is more preferably 0.005% or more. On the other hand, if the Sb content exceeds 0.200%, a soft layer is not formed near the steel sheet surface, which may lead to a decrease in energy absorption characteristics. Therefore, when Sb is contained, the Sb content is preferably 0.200% or less. The Sb content is more preferably 0.020% or less.

[0048] Sn: 0.200% or less Like Sb, Sn is an element that suppresses the diffusion of C near the steel sheet surface during annealing and is effective in controlling the formation of a soft layer near the steel sheet surface. If the soft layer increases excessively near the steel sheet surface, it becomes difficult to achieve a TS of 1180 MPa or more. It also leads to a decrease in YS. Therefore, the Sn content is preferably 0.002% or more. The Sn content is more preferably 0.005% or more. On the other hand, if the Sn content exceeds 0.200%, a soft layer is not formed near the steel sheet surface, which may lead to a decrease in energy absorption characteristics. Therefore, when Sn is contained, the Sn content is preferably 0.200% or less. The Sn content is more preferably 0.020% or less.

[0049] Cu: 1.000% or less Cu is an element that improves hardenability, so the addition of Cu produces a large amount of tempered martensite, ensuring a TS of 1180 MPa or more and a high YS. To achieve this effect, the Cu content is preferably 0.005% or more. The Cu content is more preferably 0.008% or more, and even more preferably 0.010% or more. The Cu content is more preferably 0.020% or more, and even more preferably 0.050% or more. On the other hand, if the Cu content exceeds 1.000%, the area fraction of fresh martensite increases excessively, and large amounts of coarse precipitates and inclusions may be produced. In such cases, the fresh martensite and coarse precipitates and inclusions may become the starting points for void formation during a VDA bending test, which may prevent the desired bendability of the steel sheet from being achieved. Furthermore, an increase in the area fraction of fresh martensite may introduce mobile dislocations into ferrite and bainitic ferrite, resulting in a decrease in YS. Therefore, when Cu is contained, the Cu content is preferably 1.000% or less, and more preferably 0.200% or less.

[0050] Ta: 0.100% or less Like Ti, Nb, and V, Ta increases TS and YS by forming fine carbides, nitrides, or carbonitrides during hot rolling and annealing. Additionally, Ta partially dissolves in Nb carbides and Nb carbonitrides to form complex precipitates such as (Nb, Ta)(C, N). This suppresses coarsening of precipitates and stabilizes precipitation strengthening. This further improves TS and YS. To achieve this effect, the Ta content is preferably 0.001% or more. The Ta content is more preferably 0.002% or more, and even more preferably 0.004% or more. On the other hand, if the Ta content exceeds 0.100%, large amounts of coarse precipitates and inclusions may be formed. In such cases, the amount of voids formed during VDA bending tests may increase, potentially preventing the desired bendability from being achieved. Therefore, when Ta is contained, the Ta content is preferably 0.100% or less, more preferably 0.090% or less, even more preferably 0.080% or less, and still more preferably 0.020% or less.

[0051] W: 0.500% or less. W is an element that improves hardenability, so the addition of W results in the formation of a large amount of tempered martensite, ensuring a TS of 1180 MPa or more and a high YS. To achieve this effect, the W content is preferably 0.001% or more. The W content is more preferably 0.030% or more. On the other hand, if the W content exceeds 0.500%, the area fraction of hard fresh martensite increases excessively, which may introduce mobile dislocations into ferrite and bainitic ferrite, resulting in a decrease in YS. Furthermore, fresh martensite may serve as a starting point for void generation during a VDA bending test, potentially preventing the desired bendability of the steel sheet. Therefore, when W is added, the W content is preferably 0.500% or less. The W content is more preferably 0.450% or less, and even more preferably 0.400% or less. The W content is even more preferably 0.300% or less. The W content is more preferably 0.100% or less.

[0052] Mg: 0.0200% or less. Mg is an element that effectively spheroidizes inclusions such as sulfides and oxides, improving the ultimate deformability and bendability of steel sheets. To achieve this effect, the Mg content is preferably 0.0001% or more. The Mg content is more preferably 0.0005% or more, even more preferably 0.0010% or more, and even more preferably 0.0020% or more. On the other hand, if the Mg content exceeds 0.0200%, a large amount of coarse precipitates and inclusions may be formed. In such cases, the amount of voids formed during the VDA bending test may increase, potentially making it difficult to achieve the desired bendability. Therefore, when Mg is added, the Mg content is preferably 0.0200% or less. The Mg content is more preferably 0.0180% or less, and even more preferably 0.0150% or less.

[0053] Zn: 0.0200% or less Zn is an element that effectively spheroidizes the shape of inclusions and improves the ultimate deformability and bendability of the steel sheet. To achieve this effect, the Zn content is preferably 0.0010% or more. The Zn content is more preferably 0.0020% or more, and even more preferably 0.0030% or more. On the other hand, if the Zn content exceeds 0.0200%, a large amount of coarse precipitates and inclusions may be generated. In such cases, the amount of voids generated during the VDA bending test may increase, and the desired bendability may not be achieved. Therefore, when Zn is contained, the Zn content is preferably 0.0200% or less. The Zn content is more preferably 0.0180% or less, and even more preferably 0.0150% or less.

[0054] Co: 0.0200% or less Like Zn, Co is an element that effectively spheroidizes the shape of inclusions and improves the ultimate deformability and bendability of steel sheets. To achieve this effect, the Co content is preferably 0.0010% or more. The Co content is more preferably 0.0020% or more, and even more preferably 0.0030% or more. On the other hand, if the Co content exceeds 0.0200%, a large amount of coarse precipitates and inclusions may be generated. In such cases, the amount of voids generated during the VDA bending test may increase, and the desired bendability may not be achieved. Therefore, when Co is contained, the Co content is preferably 0.0200% or less. The Co content is more preferably 0.0180% or less, and even more preferably 0.0150% or less.

[0055] Zr: 0.1000% or less Like Zn and Co, Zr is an element that effectively spheroidizes the shape of inclusions and improves the ultimate deformability and bendability of steel sheets. To achieve this effect, the Zr content is preferably 0.0010% or more. On the other hand, if the Zr content exceeds 0.1000%, a large amount of coarse precipitates and inclusions may be formed. In such cases, the amount of voids formed during the VDA bending test may increase, and the desired bendability may not be achieved. Therefore, when Zr is contained, the Zr content is preferably 0.1000% or less. The Zr content is more preferably 0.0300% or less, and even more preferably 0.0100% or less.

[0056] Ca: 0.0200% or less Ca exists as inclusions in steel. Here, if the Ca content exceeds 0.0200%, a large amount of coarse inclusions may be generated. In such a case, the amount of voids generated during the VDA bending test increases, and the desired bendability may not be achieved. Therefore, when Ca is contained, the Ca content is preferably 0.0200% or less. The Ca content is preferably 0.0020% or less. Note that the lower limit of the Ca content is not particularly limited, but the Ca content is preferably 0.0005% or more. Furthermore, due to constraints in production technology, the Ca content is more preferably 0.0010% or more.

[0057] Se: 0.0200% or less, Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0500% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, REM: 0.0200% or less. Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi and REM are all effective elements for improving the ultimate deformability and further the bendability of steel sheet. To obtain such effects, the contents of Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi and REM are each preferably 0.0001% or more. On the other hand, if the contents of Se, Te, Ge, Sr, Cs, Hf, Pb, Bi, and REM exceed 0.0200% each, or if the content of As exceeds 0.0500%, respectively, large amounts of coarse precipitates and inclusions may be formed. In such cases, the amount of voids formed during a VDA bending test may increase, and the desired bendability may not be achieved. Therefore, when at least one of Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi, and REM is contained, it is preferable that the contents of Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi, and REM are each 0.0200% or less, and the content of As is 0.0500% or less. The Se content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The Se content is more preferably 0.0180% or less, and even more preferably 0.0150% or less. The Te content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The Te content is more preferably 0.0180% or less, and even more preferably 0.0150% or less. The Ge content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The Ge content is more preferably 0.0180% or less, and even more preferably 0.0150% or less. The As content is more preferably 0.0010% or more, and even more preferably 0.0015% or more.The As content is more preferably 0.0400% or less, and even more preferably 0.0300% or less. The Sr content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The Sr content is more preferably 0.0180% or less, and even more preferably 0.0150% or less. The Cs content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The Cs content is more preferably 0.0180% or less, and even more preferably 0.0150% or less. The Hf content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The Hf content is more preferably 0.0180% or less, and even more preferably 0.0150% or less. The Pb content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The Pb content is more preferably 0.0180% or less, and even more preferably 0.0150% or less. The Bi content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The Bi content is more preferably 0.0180% or less, and even more preferably 0.0150% or less, and even more preferably 0.0100% or less. The REM content is more preferably 0.0005% or more, and even more preferably 0.0008% or more. The REM content is more preferably 0.0180% or less, and even more preferably 0.0150% or less.

[0058] In the present invention, REM refers to scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and lanthanoids ranging from lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71. The REM content in the present invention refers to the total content of one or more elements selected from the above-mentioned REM. The REM is not particularly limited, but is preferably La and / or Ce.

[0059] That is, the base steel sheet of the steel sheet of the present invention contains, in mass %, C: 0.050% or more and 0.400% or less, Si: 0.20% or more and 3.00% or less, Mn: 1.00% or more and less than 3.50%, P: 0.001% or more and 0.100% or less, S: 0.0001% or more and 0.0200% or less, Al: 0.010% or more and 2.000% or less, and N: 0.0100% or less, and optionally Nb: 0.200% or less, Ti: 0.200% or less, V: 0.200% or less, B: 0.0100% or less, Cr: 1.000% or less, Ni: 1.000% or less, Mo: 1.000% or less, Sb: 0.200% or less, Sn: 0.200% or less, Cu: 1.00 and at least one selected from the group consisting of Cr: 0.0200% or less, Ta: 0.100% or less, W: 0.500% or less, Mg: 0.0200% or less, Zn: 0.0200% or less, Co: 0.0200% or less, Zr: 0.1000% or less, Ca: 0.0200% or less, Se: 0.0200% or less, Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0500% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, and REM: 0.0200% or less, with the balance being Fe and unavoidable impurities.

[0060] Next, the steel structure of a steel sheet (base steel sheet) according to one embodiment of the present invention will be described. The structure at the 1 / 4 position of the sheet thickness of the base steel sheet is as follows: area ratio of ferrite: less than 20.0% (including 0.0%), area ratio of retained austenite: 3.0% to 15.0%, area ratio of fresh martensite: 10.0% or less (including 0.0%), total area ratio of bainitic ferrite and tempered martensite (excluding retained austenite): 45.0% to 90.0%, L F―MA / L F : 0.70 or less.

[0061] Ferrite area ratio: less than 20.0% (including 0.0%) Soft ferrite is a phase that improves ductility. However, if the ferrite area ratio increases excessively, it may become difficult to achieve a TS of 1180 MPa or more. It may also result in a decrease in YR. Therefore, the ferrite area ratio is set to less than 20.0%. The ferrite area ratio is preferably 15.0% or less. The lower limit of the ferrite area ratio is not particularly limited and may be 0.0%.

[0062] Area fraction of retained austenite: 3.0% or more and 15.0% or less From the viewpoint of obtaining good ductility, the area fraction of retained austenite is set to 3.0% or more. The area fraction of retained austenite is preferably 3.5% or more. On the other hand, if the area fraction of retained austenite increases excessively, the carbon content in the retained austenite decreases and becomes unstable. In that case, the desired YS cannot be achieved. Therefore, the area fraction of retained austenite is set to 15.0% or less. The area fraction of retained austenite is preferably 12.0% or less, and more preferably 10.0% or less.

[0063] Area fraction of fresh martensite: 10.0% or less (including 0.0%). If the area fraction of fresh martensite is excessively increased, mobile dislocations may be introduced into ferrite or bainitic ferrite, making it impossible to achieve the desired YS. Furthermore, the desired YR may not be obtained. Furthermore, fresh martensite may become the origin of void generation during a VDA bending test, which may prevent the desired bendability of the steel sheet. From the viewpoint of ensuring a high YS and good bendability of the steel sheet, the area fraction of fresh martensite is 10.0% or less, preferably 5.0% or less. The lower limit of the area fraction of fresh martensite is not particularly limited and may be 0.0%. Fresh martensite refers to as-quenched (untempered) martensite.

[0064] Total area ratio of bainitic ferrite and tempered martensite: 45.0% or more and 90.0% or less Bainitic ferrite and tempered martensite have intermediate hardness between soft ferrite and hard fresh martensite, and are important phases for ensuring good bendability of steel sheets. Bainitic ferrite is also a useful phase for obtaining an appropriate amount of retained austenite by utilizing the diffusion of C from bainitic ferrite to untransformed austenite. Tempered martensite is effective for improving TS and YS. Therefore, the total area ratio of bainitic ferrite and tempered martensite is set to 45.0% or more, preferably 50.0% or more. On the other hand, if the total area ratio of bainitic ferrite and tempered martensite increases excessively, ductility decreases. Therefore, the total area ratio of bainitic ferrite and tempered martensite is set to 90.0% or less. The total area ratio of bainitic ferrite and tempered martensite is preferably 85.0% or less. Bainitic ferrite is upper bainite with a small amount of carbides that is formed in a relatively high temperature range.

[0065] L F―MA / L F : 0.70 or less The steel structure of the base steel sheet of the steel sheet according to one embodiment of the present invention further comprises L F―MA / L F : 0.70 or less. F―MA L: length of the grain boundary on the ferrite grain boundary in contact with the MA structure (fresh martensite and / or retained austenite) F : length of the ferrite grain boundary. F―MA and L F and L are the grain boundary lengths measured in the same units. In a steel sheet having a dual-phase structure according to an embodiment of the present invention, the presence of fresh martensite introduces mobile dislocations into ferrite, making the ferrite more susceptible to yielding and reducing the YS. In particular, L F―MA / L F If L exceeds 0.70, the desired YS may not be achieved. Also, the desired YR may not be obtained. F―MA / L Fis 0.70 or less. F―MA / L F is preferably 0.68 or less, more preferably 0.65 or less. F―MA / L F The lower limit of L is not particularly limited and may be 0.00. F―MA / L F In order to make the Mn content of the austenite grains 0.70 or less, for example, by increasing the temperature from the annealing temperature at a rate of 10°C / sec or more in the rapid heating step described below, austenite can be generated around the ferrite grains by the diffusion of C alone. S The temperature is high and the austenite becomes bainitic ferrite or martensite during cooling. The martensite becomes tempered martensite during the reheating and holding process. In other words, a structure other than the hard phase (hard second phase) is generated from the austenite generated only by the diffusion of C.

[0066] The area ratio of the remaining structure other than the above is preferably 10.0% or less. The area ratio of the remaining structure is more preferably 5.0% or less. The area ratio of the remaining structure may also be 0.0%. The remaining structure is not particularly limited, and examples thereof include carbides such as lower bainite, pearlite, and cementite. The type of the remaining structure can be confirmed, for example, by observation using a scanning electron microscope (SEM).

[0067] Soft surface layer: total area ratio of structures other than ferrite is 1 / 2 or less at the 1 / 4 position of the plate thickness The base steel plate of the steel plate according to one embodiment of the present invention has a soft surface layer on the surface layer of the base steel plate. The soft surface layer contributes to suppressing the propagation of bending cracks during press forming and vehicle collisions, thereby improving the bendability and energy absorption characteristics of the steel plate. The soft surface layer means a decarburized layer, and the total area ratio of structures other than ferrite in the cross section at the 1 / 4 position of the plate thickness is defined as S A When the total area ratio of the structure other than ferrite is S A / 2 or less. Here, the soft surface layer is formed in a region of 20 μm or more from the surface of the base steel sheet in the sheet thickness direction. The region where the soft surface layer is formed is preferably 200 μm or less, more preferably 150 μm or less, and even more preferably 120 μm or less from the surface of the base steel sheet in the sheet thickness direction. The thickness of the soft surface layer is preferably 25 μm or more, and more preferably 30 μm or more. In addition, the total area ratio S of the structures other than ferrite A The position of 1 / 4 of the plate thickness of the steel plate where is measured is a non-surface soft layer (a layer that does not satisfy the conditions of the surface soft layer defined in the present invention).

[0068] Here, the area ratios of ferrite, bainitic ferrite, tempered martensite, and hard phase (hard second phase (retained austenite + fresh martensite)) at a quarter-thickness position of the base steel sheet are measured as follows. That is, a sample is cut out from the base steel sheet so that the thickness cross section parallel to the rolling direction of the base steel sheet serves as the observation surface. Next, the observation surface of the sample is mirror-polished using diamond paste. Next, the observation surface of the sample is finish-polished using colloidal silica, and then etched with 3 vol. % nital to reveal the structure. Then, using a SEM (Scanning Electron Microscope), three fields of view of 25.6 μm × 17.6 μm are photographed at the outermost layer position and the quarter-thickness position of the observation surface of the sample under conditions of an acceleration voltage of 15 kV and a magnification of 5000x. From the obtained structural image (see FIG. 1), ferrite F, bainitic ferrite BF, tempered martensite TM, and hard phase H (hard second phase (retained austenite + fresh martensite)) are identified as follows.

[0069] Ferrite: A region that is black and has a blocky shape. It contains almost no iron-based carbides. However, if iron-based carbides are contained, the area of ​​the ferrite includes the area of ​​the iron-based carbides. The same applies to bainitic ferrite and tempered martensite, which will be described later. Bainitic ferrite: A region that is black to dark gray and has a blocky or amorphous shape. It contains no iron-based carbides or a relatively small number of iron-based carbides. Tempered martensite: A region that is gray and has an amorphous shape. It contains a relatively large number of iron-based carbides. Hard phase (hard second phase (retained austenite + fresh martensite)): A region that is white to light gray and has an amorphous shape. It does not contain iron-based carbides. When the size is relatively large, the color gradually darkens as it moves away from the interface with other structures, and the interior may be dark gray. Carbides: White regions with a dotted or linear shape. They are contained within tempered martensite, bainitic ferrite, and ferrite. Remaining structures: Examples include lower bainite, pearlite, and internal oxides, and their forms are well known.

[0070] Next, the regions of each phase identified in the structural image are color-coded (quaternary imaged) using Adobe Photoshop from Adobe Systems, Inc., and the area of ​​each phase is calculated. The area of ​​each phase (total area for each phase) is divided by the area of ​​the observation region (25.6 μm × 17.6 μm) and multiplied by 100 to calculate the value for three fields of view. The average of these values ​​is then used as the area ratio of each phase (ferrite, bainitic ferrite, tempered martensite, and hard second phase).

[0071] The area fraction of retained austenite is measured as follows. The base steel sheet is mechanically ground in the thickness direction (depth direction) to a position one-quarter of the sheet thickness, and then chemically polished with oxalic acid to obtain an observation surface. The observation surface is then observed by X-ray diffraction. MoKα rays are used as the incident X-rays, and the ratios of the diffraction intensities of the (200), (220), and (311) planes of fcc iron (austenite) to the diffraction intensities of the (200), (211), and (220) planes of bcc iron are calculated, and the volume fraction of retained austenite is calculated from the ratio of the diffraction intensities of each plane. The retained austenite is then considered to be three-dimensionally homogeneous, and the volume fraction of retained austenite is taken as the area fraction of retained austenite.

[0072] The area fraction of fresh martensite is calculated by subtracting the area fraction of retained austenite from the area fraction of the hard phase (hard second phase) calculated as described above: [Area fraction of fresh martensite (%)] = [Area fraction of hard second phase (%)] - [Area fraction of retained austenite (%)]

[0073] The area ratio of the remaining structure is calculated by subtracting the area ratio of ferrite, the area ratio of bainitic ferrite, the area ratio of tempered martensite, and the area ratio of the hard phase (hard second phase) calculated as described above from 100.0%: [Area ratio of remaining structure (%)] = 100.0 - [Area ratio of ferrite (%)] - [Area ratio of bainitic ferrite (%)] - [Area ratio of tempered martensite (%)] - [Area ratio of hard second phase (%)]

[0074] For measuring the structure of the soft surface layer, if a zinc-plated layer is formed on the steel sheet, first peel off the zinc-plated layer, and measure the structure in the same manner as at the 1 / 4 position in the sheet thickness direction at 1 μm intervals from a position 1 μm from the surface of the base steel sheet in the sheet thickness direction to a position 100 μm in the sheet thickness direction, and then measure at 20 μm intervals to the center of the sheet thickness.

[0075] Also, L F―MA , L FThe L is measured as follows: In a structural image (see, for example, FIG. 1), ferrite and hard phases (hard second phases) are identified as described above. Then, the ferrite and hard phases (hard second phases) are manually extracted, and the L is measured using the open-source ImageJ. F―MA , L F Specifically, the ferrite grain boundary L is calculated using the above-mentioned quaternized structure image and the object function of Adobe Illustrator. F and the grain boundary L that contacts the ferrite and martensite structure (MA structure: fresh martensite + retained austenite). F―MA Draw a curve along each line and measure the length of the curve. F―MA L F Calculate the value divided by and take the average value as L F―MA / L F Let's say.

[0076] Next, the mechanical properties of the steel plate according to one embodiment of the present invention will be described.

[0077] Tensile strength (TS): 1180 MPa or more and less than 1470 MPa The tensile strength TS of the steel plate according to one embodiment of the present invention is 1180 MPa or more and less than 1470 MPa. The yield stress (YS), yield ratio (YR), total elongation (El), bendability and energy absorption characteristics of the steel plate according to one embodiment of the present invention are as described above.

[0078] The tensile strength (TS), yield stress (YS), yield ratio (YR) and total elongation (El) are measured by a tensile test in accordance with JIS Z 2241 (2011) described later in the examples. The bendability and energy absorption characteristics of the steel sheet are measured by a VDA bending test described later in the examples.

[0079] Galvanized Layer A steel sheet according to one embodiment of the present invention may have a galvanized layer formed on the base steel sheet, and this galvanized layer may be provided on only one surface of the base steel sheet, or on both surfaces.

[0080] The galvanized layer referred to here refers to a plated layer containing Zn as a main component (Zn content: 50.0 mass % or more), and examples thereof include a hot-dip galvanized layer, a galvannealed hot-dip galvanized layer, and an electrogalvanized layer.

[0081] Here, the hot-dip galvanized layer is preferably composed of, for example, Zn, 20.0 mass% or less Fe, and 0.001 mass% to 1.0 mass% Al. The hot-dip galvanized layer may optionally contain one or more elements selected from the group consisting of Pb, Sb, Si, Sn, Mg, Mn, Ni, Cr, Co, Ca, Cu, Li, Ti, Be, Bi, and REM in a total amount of 0.0 mass% to 3.5 mass%. The Fe content of the hot-dip galvanized layer is more preferably less than 7.0 mass%. The remainder other than the above elements is unavoidable impurities.

[0082] The galvannealed layer is preferably composed of, for example, Zn, 20% by mass or less of Fe, and 0.001% by mass to 1.0% by mass or less of Al. The galvannealed layer may optionally contain one or more elements selected from the group consisting of Pb, Sb, Si, Sn, Mg, Mn, Ni, Cr, Co, Ca, Cu, Li, Ti, Be, Bi, and REM in a total amount of 0.0% by mass to 3.5% by mass. The Fe content of the galvannealed layer is more preferably 7.0% by mass or more, and even more preferably 8.0% by mass or more. The Fe content of the galvannealed layer is more preferably 15.0% by mass or less, and even more preferably 12.0% by mass or less. The remainder other than the above elements is unavoidable impurities.

[0083] The electrogalvanized layer is preferably composed of, for example, Zn and 9.0 mass % to 25.0 mass % Ni, the remainder being unavoidable impurities.

[0084] In addition, the coating weight of the hot-dip galvanized layer and the galvannealed hot-dip galvanized layer per side is not particularly limited, but is preferably 20 g / m 2The coating weight of the hot-dip galvanized layer and the galvannealed hot-dip galvanized layer per side is preferably 80 g / m or more. 2 The plating weight of the electrogalvanized layer per side is not particularly limited, but is preferably 10 g / m or less. 2 The plating weight of the electrogalvanized layer on one side is preferably 100 g / m or more. 2 It is preferable to do the following:

[0085] The coating weight of a zinc-coated layer (hot-dip galvanized layer, galvannealed hot-dip galvanized layer, electrogalvanized layer) is measured as follows. That is, a treatment solution is prepared by adding 0.6 g of a corrosion inhibitor for Fe (Ivit 700BK (registered trademark) manufactured by Asahi Chemical Industry Co., Ltd.) to 1 L of a 10 mass % aqueous hydrochloric acid solution. Next, a steel sheet to be used as a test material is immersed in the treatment solution to dissolve the zinc-coated layer. The mass loss of the test material before and after dissolution is measured, and this value is divided by the surface area of ​​the base steel sheet (the surface area of ​​the part that was covered with the coating) to determine the coating weight (g / m 2 ) is calculated.

[0086] The thickness of the steel plate according to one embodiment of the present invention is not particularly limited, but is preferably more than 0.8 mm, more preferably 0.9 mm or more. The thickness is even more preferably 1.0 mm or more, and most preferably 1.2 mm or more. The thickness of the steel plate is preferably 3.5 mm or less. The thickness is more preferably 2.3 mm or less. The width of the steel plate according to the present invention is not particularly limited, but is preferably 500 mm or more, and more preferably 750 mm or more. The width of the steel plate is preferably 1600 mm or less, and more preferably 1450 mm or less.

[0087] 2. Method for Manufacturing Steel Sheet Next, a method for manufacturing a steel sheet according to one embodiment of the present invention will be described.

[0088] A method for producing a steel sheet according to one embodiment of the present invention includes a hot rolling process in which a steel slab having the above-described chemical composition is hot-rolled to produce a hot-rolled steel sheet; a pickling process in which the hot-rolled steel sheet is pickled; an annealing process in which the steel sheet after the pickling process or the steel sheet after the cold rolling process is heated and annealed under conditions of an annealing temperature of 720°C to 860°C, a holding time of 20 seconds or more, and a dew point of -10°C or higher; and a rapid heating process in which the temperature is raised from the annealing temperature to a temperature of annealing temperature + 10°C or higher under conditions of a heating rate of 10°C / second or higher. The method includes a rapid heating step of heating the steel sheet to a temperature range of 100°C or higher and 300°C or lower, a cooling step of cooling the steel sheet after the rapid heating step to a cooling stop temperature of 100°C or higher and 300°C or lower, and a reheating and holding step of heating the steel sheet after the cooling step to a tempering temperature of 460°C or lower and holding the steel sheet in the temperature range for a tempering time of 10 seconds or higher and 2000 seconds or lower, or may further include a cold rolling step of cold rolling the steel sheet after the pickling step and before the annealing step at a rolling reduction of 20% or higher and 80% or lower to obtain a cold-rolled steel sheet. The passing speed LS (m / min) of the steel sheet in the annealing step preferably satisfies the following formula (1): 3.0 / (t×W×4.716×10 ―4 )<LS<390.0 / (t×W×4.716×10 ―4 ) Formula (1) t: plate thickness (mm) after pickling process and before annealing process, W: plate thickness (mm) after pickling process and before annealing process. Note that, unless otherwise specified, the above temperatures refer to the surface temperatures of the steel slab and the steel plate.

[0089] First, a steel slab having the above-described composition is prepared. For example, a steel material is melted to obtain molten steel having the above-described composition. The melting method is not particularly limited, and known melting methods such as converter melting and electric furnace melting can be used. Next, the obtained molten steel is solidified to obtain a steel slab. The method for obtaining a steel slab from molten steel is not particularly limited, and for example, a continuous casting method, an ingot casting method, or a thin slab casting method can be used. From the viewpoint of preventing macrosegregation, it is preferable to adopt a continuous casting method as a method for obtaining a steel slab from molten steel.

[0090] (Hot Rolling Step) Next, in the hot rolling step, the steel slab is hot rolled to produce a hot-rolled steel sheet. Hot rolling may be performed using an energy-saving process. Examples of the energy-saving process include direct rolling (a method in which the steel slab is not cooled to room temperature, but is charged into a heating furnace as a hot slab and hot-rolled), direct rolling (a method in which the steel slab is briefly kept at a constant temperature and then immediately rolled), etc.

[0091] The hot rolling conditions are not particularly limited, and can be, for example, the following conditions. That is, the steel slab is once cooled to room temperature, and then reheated and rolled. The slab heating temperature (reheating temperature) is preferably 1100°C or higher from the viewpoint of dissolving carbides and reducing the rolling load. Furthermore, in order to prevent an increase in scale loss, the slab heating temperature is preferably 1300°C or lower. The slab heating temperature is based on the temperature of the steel slab surface.

[0092] Next, the steel slab is subjected to rough rolling according to a conventional method to obtain a rough-rolled plate (hereinafter also referred to as a sheet bar). The sheet bar is then subjected to finish rolling to obtain a hot-rolled steel plate. When the slab heating temperature is low, it is preferable to heat the sheet bar using a bar heater or the like before finish rolling in order to prevent problems during finish rolling. The finish rolling temperature is preferably 800°C or higher to reduce the rolling load. Furthermore, if the reduction rate in the unrecrystallized austenite state becomes high, an abnormal structure elongated in the rolling direction may develop, which may reduce the workability of the annealed sheet. Furthermore, by setting the finish rolling temperature to 800°C or higher, the steel structure at the hot-rolled steel plate stage, and ultimately the steel structure of the final product, tends to become uniform. A non-uniform steel structure tends to reduce bendability. On the other hand, if the finish rolling temperature exceeds 950°C, the amount of oxide (scale) generated increases. As a result, the interface between the base steel and the oxide may become rough, which may deteriorate the surface quality of the steel sheet after pickling and cold rolling. Furthermore, the crystal grains may become coarse, which may cause a decrease in the strength and bendability of the steel sheet. Therefore, the finish rolling temperature is preferably set in the range of 950°C or less. For these reasons, the finish rolling temperature is preferably set in the range of 800°C or more and 950°C or less.

[0093] After finish rolling, the hot-rolled steel sheet is coiled. The coiling temperature is preferably 450°C or higher, and 750°C or lower.

[0094] Note that the sheet bars may be joined together during hot rolling and continuous finish rolling may be performed. The sheet bars may also be wound up before finish rolling. Furthermore, in order to reduce the rolling load during hot rolling, some or all of the finish rolling may be performed as lubricated rolling. Performing lubricated rolling is also effective from the viewpoint of uniforming the shape and material properties of the steel sheet. Note that the friction coefficient during lubricated rolling is preferably in the range of 0.10 to 0.25. In a hot rolling process (hot rolling process) including rough rolling and finish rolling, a steel slab is generally made into a sheet bar by rough rolling and then made into a hot-rolled steel sheet by finish rolling. However, depending on the mill capacity, etc., such classification is not essential as long as the desired size is achieved.

[0095] (Pickling process) The hot-rolled steel sheet after the hot rolling process is pickled. Pickling can remove oxides from the steel sheet surface, ensuring good chemical conversion treatability and plating quality. Pickling may be carried out once or multiple times. The pickling conditions are not particularly limited, and may be carried out in accordance with conventional methods.

[0096] (Cold Rolling Process) Next, if necessary, the hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet. Cold rolling is performed, for example, by multi-pass rolling requiring two or more passes, such as tandem multi-stand rolling or reverse rolling. The cold-rolling reduction (cumulative reduction) is not particularly limited, but is preferably 20% or more. Furthermore, the cold-rolling reduction is preferably 80% or less. If the cold-rolling reduction is less than 20%, the steel structure is likely to become coarse and non-uniform during the annealing process, which may result in reduced TS and bendability in the final product. On the other hand, if the cold-rolling reduction exceeds 80%, the steel sheet is likely to have a defective shape and the amount of zinc coating may become non-uniform. Optionally, the cold-rolled steel sheet obtained after cold rolling may be pickled.

[0097] (Annealing step) Next, in one embodiment of the present invention, after the pickling step (or after the cold rolling step if cold rolling is performed), the steel sheet obtained as described above is heated and annealed at an annealing temperature of 720°C or higher and 860°C or lower for a holding time (annealing time) of 20 seconds or longer. Note that the number of annealing steps may be two or more, but one step is preferred from the viewpoint of energy efficiency. The annealing step is a step including this heating treatment and soaking treatment.

[0098] Annealing temperature: 720°C or higher and 860°C or lower When the annealing temperature is lower than 720°C, the austenite generation rate during heating in the two-phase region of ferrite and austenite becomes insufficient. As a result, the area ratio of ferrite increases excessively after annealing, resulting in a decrease in YS. In addition, the amount of fresh martensite increases due to excessive carbon concentration in austenite during annealing, and L F―MA / L F exceeds 0.70, and the desired YS cannot be achieved. Furthermore, there is a risk that the bendability of the steel sheet cannot be achieved. Furthermore, it becomes difficult to achieve a TS of 1180 MPa or more. On the other hand, if the annealing temperature exceeds 860°C, the proportion of ferrite during annealing becomes insufficient, the diffusion of C near the steel sheet surface is suppressed, and the desired soft surface layer is not formed. Therefore, the annealing temperature is set to 720°C or more and 860°C or less. The annealing temperature is preferably 850°C or less. The annealing temperature is the maximum temperature reached in the annealing process.

[0099] Holding time (annealing time): 20 seconds or more If the holding time (annealing time) is less than 20 seconds, the austenite generation rate during heating in the two-phase region of ferrite and austenite becomes insufficient. As a result, the area ratio of ferrite increases excessively after annealing, which may result in a decrease in YS. Also, the YR decreases. In addition, the amount of fresh martensite increases due to excessive carbon concentration in austenite during annealing, resulting in a decrease in L. F―MA / L FIf the value exceeds 0.70, the desired YS may not be obtained. Furthermore, the YR may decrease. Furthermore, the bendability of the steel sheet may not be achieved. Furthermore, it may become difficult to achieve a TS of 1180 MPa or more. Therefore, the holding time (annealing time) is set to 20 seconds or more. The holding time is preferably 30 seconds or more, more preferably 50 seconds or more. While the upper limit of the holding time is not particularly limited, the holding time is preferably 900 seconds or less, more preferably 800 seconds or less. The holding time refers to the holding time in a temperature range of (annealing temperature -40°C) or more and the annealing temperature or less. In other words, the holding time includes not only the holding time at the annealing temperature, but also the residence time in a temperature range of (annealing temperature -40°C) or more and the annealing temperature or less during heating and cooling before and after reaching the annealing temperature.

[0100] Dew point of atmosphere in annealing step (annealing atmosphere): -10°C or higher In one embodiment of the present invention, the dew point of the atmosphere in the annealing step (annealing atmosphere) is -10°C or higher. By performing annealing in the annealing step with a dew point of the annealing atmosphere of -10°C or higher, the decarburization reaction is promoted and a soft surface layer having a desired thickness can be formed. The dew point of the annealing atmosphere in the annealing step is preferably -5°C or higher, more preferably 0°C or higher, and even more preferably higher than 5°C. There is no particular upper limit for the dew point of the annealing atmosphere in the annealing step, but in order to improve plating adhesion when a zinc-plated layer is formed, the dew point of the annealing atmosphere in the annealing step is preferably 30°C or lower.

[0101] 3.0 / (t×W×4.716×10 ―4 )<LS<390.0 / (t×W×4.716×10 ―4 ) Equation (1) In the present invention, from the viewpoint of production efficiency, it is preferable that the steel sheet threading speed LS (m / min) in the annealing process satisfies equation (1). In equation (1), t: sheet thickness (mm) after the pickling process and before the annealing process, W: sheet width (mm) after the pickling process and before the annealing process. The production efficiency can be defined as E, which is expressed by the following equation (2): E (ton / h) = LS x t x W x ρ x 60 x 10 ―6 ...Equation (2) In equation (2), t: plate thickness (mm), W: plate width (mm), ρ: specific gravity of iron (ton / m 3), and ρ=7.86 (ton / m 3 ), where E is preferably more than 3.0 ton / h and less than 390.0 ton / h. Based on this formula (2), the above formula (1) can be derived. If E is 3.0 ton / h or less, a soft surface layer is excessively formed during annealing, making it difficult to achieve a TS of 1180 MPa or more. This may also lead to a decrease in YS. On the other hand, if E is 390.0 ton / h or more, it becomes difficult to form a desired soft surface layer during annealing, making it difficult to achieve the bendability of the steel sheet. Therefore, E is preferably more than 3.0 ton / h and less than 390.0 ton / h. Furthermore, E is more preferably 16.0 ton / h or more. Furthermore, E is more preferably 190.0 ton / h or less. From the above, LS (m / min) can be calculated by the following formula: 3.0 / (t×W×4.716×10 ―4 ) or more. LS (m / min) is preferably 16.0 / (t×W×4.716×10 ―4 ) or more. LS (m / min) is 390.0 / (t×W×4.716×10 ―4 LS (m / min) is preferably less than 190.0 / (t×W×4.716×10 ―4 ) or less is more preferable.

[0102] The sheet passing speed LS (m / min) is calculated by dividing the distance (m) traveled by the steel sheet in the annealing process by the time (min) required for the steel sheet to be transported in the annealing process.

[0103] A radiant tube furnace is generally used as the heat treatment furnace for the annealing process. The annealing temperature is obtained using a thermometer that measures the surface temperature of the steel sheet. The temperature measurement method is not particularly limited, but for example, a radiation thermometer that measures the temperature by sensing infrared rays emitted by the steel sheet is suitable. In the case of a radiation thermometer, since it may be affected by reflected light of infrared rays emitted by the surrounding furnace body, a cover may be provided between the measurement part of the radiation thermometer and the detection part of the steel sheet. Furthermore, since it may be affected by the emissivity of the steel sheet surface, a multi-reflection measurement method that utilizes the wedge-shaped space between the transport roll in the furnace and the steel sheet may be adopted.

[0104] (Rapid Heating Step) In one embodiment of the present invention, after the annealing step, the steel sheet obtained as described above is rapidly heated from the annealing temperature to a temperature 10°C higher than the annealing temperature at a heating rate of 10°C / sec or more. When annealing is performed two or more times in the annealing step described above, the treatment in the rapid heating step performed after annealing may also be performed two or more times, but the treatment in the rapid heating step may be performed only once.

[0105] Heating rate: 10°C / sec or more In one embodiment of the present invention, the heating rate from the annealing temperature to the temperature reached in the rapid heating step described below is 10°C / sec or more. By setting the heating rate to 10°C / sec or more, the diffusion of Mn from ferrite to austenite is suppressed, and austenite can be generated only by the diffusion of C. Such austenite contains Mn. S The temperature rise rate is high, and the material changes to bainitic ferrite or martensite during cooling. The martensite changes to tempered martensite during the reheating and holding process. In other words, by increasing the temperature rise rate to 10°C / sec or more, the L F―MA / L F can be made 0.70 or less, thereby improving YS. Furthermore, YR can also be improved. Furthermore, production efficiency can be improved. Therefore, the heating rate from the annealing temperature to the temperature reached in the rapid heating step is set to 10°C / s or more. The heating rate is more preferably 30°C / s or more. On the other hand, if the heating rate exceeds 300°C / s, there is a concern that the steel sheet may be buckled and deformed due to thermal stress, and local high-temperature areas may occur in the sheet width direction, making it difficult to maintain uniformity. Therefore, the heating rate in the rapid heating step is preferably 300°C / s or less, more preferably 150°C / s or less.

[0106] Rapid heating process temperature: Annealing temperature + 10°C or more When the rapid heating process temperature is less than the annealing temperature + 10°C, the generation of austenite is insufficient by the diffusion of C alone, and L F―MA / L Fmay exceed 0.70, resulting in a decrease in YS. Furthermore, YR decreases. Therefore, the temperature reached in the rapid heating step is set to annealing temperature + 10°C or higher. The temperature reached in the rapid heating step is preferably annealing temperature + 30°C or higher, and more preferably annealing temperature + 40°C or higher. There is no particular upper limit for the temperature reached in the rapid heating step, but from the viewpoint of production efficiency, it is preferably set to less than annealing temperature + 100°C, and more preferably annealing temperature + 90°C or lower.

[0107] The induction heating (IH) device in the rapid heating step rapidly heats the steel sheet by adjusting its output so that the temperature of the steel sheet is within the annealing temperature +10°C or more (preferably, 740°C or more and 940°C or less). Furthermore, when heating within this temperature range, the induction heating (IH) device is preferably a transverse type. The appropriate rapid heating temperature varies depending on the chemical composition of the steel sheet. Therefore, it is preferable to predict a suitable temperature range in advance by measurement, calculation, or simulation and set it taking into account the temperature of the steel sheet in the annealing step. The temperature reached in the rapid heating step can be measured using a thermometer that measures the surface temperature of the steel sheet. The temperature measurement method is not particularly limited, but a radiation thermometer that measures the temperature by sensing infrared rays emitted by the steel sheet is suitable. In the case of a radiation thermometer, since it may be affected by reflected light of infrared rays emitted by the surrounding furnace body, a cover may be provided between the measurement unit of the radiation thermometer and the detection unit of the steel sheet. Furthermore, since it may be affected by the emissivity of the steel sheet surface, a multi-reflection measurement method utilizing a wedge-shaped space between the transport roll in the furnace and the steel sheet may be adopted. It is also desirable to use a scanning radiation thermometer to measure the temperature at each position in the width direction of the steel plate.

[0108] (Holding step (preferable requirement)) After the rapid heating step and before the cooling step, if necessary, a holding step may be performed in which the steel sheet is held in a temperature range of 400°C or more and 600°C or less (hereinafter also referred to as a holding temperature range) for less than 80 seconds.

[0109] Holding time in the holding temperature range: less than 80 seconds During the holding step, bainitic ferrite is generated, and C diffuses from the generated bainitic ferrite to the untransformed austenite adjacent to the bainitic ferrite. As a result, a predetermined amount of area fraction of retained austenite is secured. Here, if the holding time in the holding temperature range is 80 seconds or longer, the area fraction of bainitic ferrite may increase excessively, resulting in a decrease in YS. Furthermore, excessive diffusion of C from bainitic ferrite to untransformed austenite may occur, causing the area fraction of retained austenite to exceed 15.0%, potentially preventing the desired YS and bendability from being achieved. Therefore, the holding time in the holding temperature range is preferably less than 80 seconds. The holding time in the holding temperature range is more preferably less than 60 seconds.

[0110] (Cooling Step) Next, the steel sheet after the rapid heating step (or after the holding step if the steel sheet is subjected to the holding step) is cooled to a cooling stop temperature of 100°C or higher and 300°C or lower.

[0111] Cooling stop temperature: 100°C or higher and 300°C or lower. The cooling process is necessary to control the area fraction of tempered martensite and the area fraction of retained austenite generated in the subsequent reheating and holding process within a predetermined range. Here, if the cooling stop temperature is lower than 100°C, the untransformed austenite present in the steel during the cooling process is almost entirely transformed into martensite. This results in an excessive increase in the area fraction of tempered martensite, making it difficult to obtain an area fraction of retained austenite of 3.0% or higher, and reducing ductility. On the other hand, if the cooling stop temperature exceeds 300°C, the area fraction of tempered martensite decreases and the area fraction of fresh martensite increases. As a result, the desired YS may not be obtained. Furthermore, the YR may decrease. Furthermore, bendability may not be achieved. Therefore, the cooling stop temperature is set to 100°C or higher and 300°C or lower. The cooling stop temperature is preferably 120°C or higher. The cooling stop temperature is preferably 280°C or lower.

[0112] (Galvanizing Process (Hot-Dip Galvanizing Process, Alloying Process)) During the cooling process, after the cooling process and before the reheating and holding process, or after the reheating and holding process, the steel sheet may be subjected to a galvanizing process (hot-dip galvanizing, or further to a galvannealing hot-dip galvanizing process). By performing the galvanizing process, a galvanized steel sheet can be obtained. Examples of the galvanizing process here include a hot-dip galvanizing process and a galvannealing process (hot-dip galvanizing process and alloying process). When the galvanizing process is performed during the cooling process, it is preferable to perform the galvanizing process after cooling the steel sheet to a bath temperature of 440 to 500°C. By performing the hot-dip galvanizing process on the steel sheet, a hot-dip galvanized steel sheet can be obtained, and by further performing an alloying process, a galvannealed hot-dip galvanized steel sheet can be obtained. Hereinafter, the hot-dip galvanizing process and the alloying process will also be collectively referred to as the galvannealing hot-dip galvanizing process.

[0113] In the case of hot-dip galvanizing, it is preferable to immerse the steel sheet in a hot-dip galvanizing bath at 440°C or higher and 500°C or lower, and then adjust the coating weight by gas wiping or the like. The hot-dip galvanizing bath is not particularly limited as long as it provides the above-mentioned composition of the zinc coating layer, but it is preferable to use a plating bath with a composition containing 0.10 mass% or more of Al, with the balance consisting of Zn and unavoidable impurities. The Al content is preferably 0.23 mass% or lower.

[0114] Furthermore, in the case of alloying hot-dip galvanizing treatment, after performing the hot-dip galvanizing treatment as described above, it is preferable to perform alloying treatment by heating the galvanized steel sheet to an alloying temperature of 450°C or higher. The alloying temperature is preferably 600°C or lower. If the alloying temperature is lower than 450°C, the Zn-Fe alloying rate will be slow, and alloying may become difficult. On the other hand, if the alloying temperature exceeds 600°C, untransformed austenite will transform to pearlite, making it difficult to achieve a TS of 1180 MPa or higher, and ductility will decrease. The alloying temperature is more preferably 470°C or higher. Furthermore, the alloying temperature is more preferably 570°C or lower.

[0115] The coating weight of both the hot-dip galvanized steel sheet (GI) and the galvannealed steel sheet (GA) was 20 g / m per side. 2 The coating weight of the zinc plating layer on one side is preferably 80 g / m or more. 2 It is preferable that the plating thickness is set to the following: The plating thickness can be adjusted by gas wiping or the like.

[0116] (Reheating and Holding Step) Next, the steel sheet is reheated to a tempering temperature of 460°C or lower (hereinafter also referred to as the reheating temperature range), and the steel sheet is held in the tempering temperature range of 460°C or lower for a tempering time of 10 seconds to 2000 seconds. This tempers the martensite present in the steel at the end of the cooling step. In addition, the C supersaturated in the martensite is diffused into the untransformed austenite, thereby generating austenite that is stable at room temperature, i.e., retained austenite.

[0117] Tempering temperature (reheating temperature): 460°C or less. If the tempering temperature (reheating temperature) exceeds 460°C, the martensite present in the steel at the end of the cooling process will be excessively tempered, making it difficult to achieve a TS of 1180 MPa or more. Furthermore, the untransformed austenite present in the steel at the end of the cooling process will decompose into carbides (pearlite), resulting in reduced ductility. Therefore, the tempering temperature (reheating temperature) is set to 460°C or less. The tempering temperature is the maximum temperature reached during the reheating and holding process. The tempering temperature is preferably 450°C or less, and more preferably 440°C or less. While there is no particular lower limit for the tempering temperature (reheating temperature), if the temperature is 300°C or less, the martensite present in the steel at the end of the cooling process will not be sufficiently tempered, resulting in an excessive increase in fresh martensite. As a result, the desired YS will not be achieved. Furthermore, there is a risk that the bendability will not be achieved. Therefore, the tempering temperature is preferably above 300°C, more preferably above 320°C.

[0118] Tempering time (holding time) in the reheating temperature range: 10 seconds or more and 2000 seconds or less. If the tempering time (holding time) in the reheating temperature range is less than 10 seconds, the martensite present in the steel at the end of the cooling process will not be sufficiently tempered, resulting in an excessive increase in fresh martensite. Furthermore, the coarsening of carbides in the tempered martensite may not proceed sufficiently, resulting in the density of carbides in the tempered martensite exceeding a predetermined amount. As a result, the desired YS may not be achieved. Furthermore, the YR may decrease. Furthermore, the bendability may not be achieved. On the other hand, if the tempering time (holding time) in the reheating temperature range exceeds 2000 seconds, the martensite present in the steel at the end of the cooling process will be excessively tempered, making it difficult to achieve a TS of 1180 MPa or more. Furthermore, the untransformed austenite present in the steel at the end of the second cooling process will decompose into carbides (pearlite), resulting in a decrease in ductility. Therefore, the tempering time (holding time) in the reheating temperature range is set to 10 seconds or more and 2000 seconds or less. The tempering time is preferably 20 seconds or more, more preferably 30 seconds or more. The tempering time is preferably 1000 seconds or less, more preferably 900 seconds or less. The tempering time (holding time) in the reheating temperature range includes not only the holding time at the reheating temperature, but also the residence time in that temperature range during heating and cooling before and after reaching the reheating temperature.

[0119] The cooling conditions after holding in the reheating temperature range are not particularly limited and may be conventional. Examples of cooling methods that can be used include gas jet cooling, mist cooling, roll cooling, water cooling, and air cooling. From the viewpoint of preventing surface oxidation, the material is preferably cooled to 50°C or less after holding in the reheating temperature range, and more preferably to room temperature. The average cooling rate after holding in the reheating temperature range is preferably, for example, 1°C / second or more. Preferably, the average cooling rate is 50°C / second or less.

[0120] (Zinc plating step (electrogalvanizing step)) After cooling to room temperature, an electrogalvanizing treatment may be performed. By subjecting the steel sheet to electrogalvanizing treatment, an electrogalvanized steel sheet can be obtained. When electrogalvanizing the steel sheet surface, the treatment conditions for the electrogalvanizing treatment are not particularly limited, and may be performed in accordance with a conventional method.

[0121] The steel sheet obtained as described above may further be subjected to temper rolling. If the temper rolling reduction exceeds 2.00%, the yield stress increases, which may result in a decrease in dimensional accuracy when the steel sheet is formed into a component. Therefore, the temper rolling reduction is preferably 2.00% or less. The lower limit of the temper rolling reduction is not particularly limited, but is preferably 0.05% or more from the viewpoint of productivity. Temper rolling may be performed on an apparatus continuous with the annealing apparatus for carrying out the above-mentioned steps (online), or may be performed on an apparatus discontinuous with the annealing apparatus for carrying out the steps (offline). The number of times temper rolling may be one, two, or more. As long as an elongation rate equivalent to that of temper rolling can be imparted, rolling using a leveler or the like may also be used.

[0122] The conditions other than those mentioned above are not particularly limited, and may be those according to conventional methods.

[0123] [3. Member] Next, a member according to one embodiment of the present invention will be described. The member according to one embodiment of the present invention is a member made using (using as a raw material) the above-mentioned steel plate. For example, the raw material steel plate is subjected to at least one of forming and joining to form a member. Here, the above-mentioned steel plate has a TS of 1180 MPa or more, a high YS, a high YR, and excellent ductility, bendability, and energy absorption properties. Therefore, the member according to one embodiment of the present invention has high strength and excellent impact resistance properties. Therefore, the member according to one embodiment of the present invention is particularly suitable for application as an impact energy absorbing member used in the automotive field.

[0124] [4. Manufacturing Method of Member] Next, a manufacturing method of a member according to one embodiment of the present invention will be described. The manufacturing method of a member according to one embodiment of the present invention includes a step of subjecting the above-mentioned steel plate (for example, a steel plate manufactured by the above-mentioned manufacturing method of steel plate) to at least one of forming and joining to form a member. Here, the forming method is not particularly limited, and for example, a general processing method such as press working can be used. Furthermore, the joining method is also not particularly limited, and for example, general welding such as spot welding, laser welding, and arc welding, rivet joining, caulking joining, etc. can be used. Note that the forming conditions and joining conditions are not particularly limited, and may be in accordance with conventional methods.

[0125] Steel materials having the chemical compositions shown in Table 1 (the balance being Fe and unavoidable impurities) were melted in a converter and then cast into steel slabs by continuous casting. In Table 1, "-" indicates the content of unavoidable impurities.

[0126] The obtained steel slabs were heated to 1200°C, and after heating, the steel slabs were subjected to hot rolling consisting of rough rolling and finish rolling at a finish rolling temperature of 900°C to obtain hot-rolled steel sheets. Next, except for No. 67, the obtained hot-rolled steel sheets were subjected to pickling and cold rolling (reduction: 50%) to obtain cold-rolled steel sheets with the thicknesses shown in Table 3. Next, the obtained cold-rolled steel sheets were subjected to treatments in the annealing step, rapid heating step, cooling step, galvanizing step, and reheating and holding step under the conditions shown in Table 2 to obtain steel sheets (galvanized steel sheets). Note that No. 66 was subjected to treatment in the holding step after the rapid heating step and before the cooling step. The conditions in this holding step were a holding temperature of 480°C and a holding time of 60 seconds.

[0127] Here, the galvanizing process involved hot-dip galvanizing, galvannealed galvanizing, or electrogalvanized processing to obtain hot-dip galvanized steel sheets (hereinafter also referred to as GI), galvannealed hot-dip galvanized steel sheets (hereinafter also referred to as GA), or electrogalvanized steel sheets (hereinafter also referred to as EG). The hot-dip galvanizing and galvannealed galvanizing processes were performed after the cooling process and before the reheating and holding process, and the electrogalvanizing process was performed after the reheating and holding process. In Table 2, the types of plating processes are also indicated as "GI," "GA," and "EG." In Table 2, GI and EG steel sheets were not subjected to alloying treatment, so the alloying temperature is indicated as "-." In Table 2, cold-rolled steel sheets obtained without undergoing zinc plating in the zinc plating process are indicated as "CR."

[0128] The galvanizing bath temperature was 470°C for all of the production of EG, GI, and GA. The galvanizing coating weight was 10 to 100 g / m when producing EG. 2 When manufacturing GI, the weight is 45 to 72 g / m per side. 2 When manufacturing GA, the thickness is 45 g / m per side. 2 The zinc plating layers of the finally obtained zinc-plated steel sheets had the following compositions: GI: 0.1 to 1.0 mass% Fe, 0.2 to 0.33 mass% Al, and the balance being Zn and unavoidable impurities; GA: 8.0 to 12.0 mass% Fe, 0.1 to 0.23 mass% Al, and the balance being Zn and unavoidable impurities; EG: 9.0 to 25.0 mass% Ni, and the balance being Zn and unavoidable impurities. The zinc plating layers were formed on both sides of the base steel sheet in all cases.

[0129] Using the obtained steel sheet, the steel structure of the base steel sheet was identified in the manner described above. The measurement results are shown in Table 3. In Table 3, F is ferrite, BF is bainitic ferrite, TM is tempered martensite, RA is retained austenite, FM is fresh martensite, LB is lower bainite, and θ is carbide. In addition, in the manner described above, the surface layer in which the total area ratio of structures other than ferrite was ½ or less at the ¼ position in the sheet thickness was determined to be the soft surface layer.

[0130] Further, a tensile test and a VDA bending test were carried out according to the following procedures, and the tensile strength (TS), yield stress (YS), yield ratio (YR), total elongation (El), limit bending angle (α) in the VDA bending test, amount of energy absorbed in bending deformation, and production efficiency (E) were evaluated according to the following criteria.

[0131] ・TS 〇 (pass): 1180 MPa or more and less than 1470 MPa × (fail): less than 1180 MPa or 1470 MPa or more

[0132] YS ◯ (Pass): (A) If 1180MPa≦TS<1320MPa, then 750MPa≦YS (B) If 1320MPa≦TS, then 850MPa≦YS × (Fail): (A) If 1180MPa≦TS<1320MPa, then 750MPa>YS (B) If 1320MPa≦TS, then 850MPa>YS

[0133] ・YR 〇 (pass): 0.70 or more × (fail): less than 0.70

[0134] El ◯ (Pass): (A) If 1180 MPa ≦ TS < 1320 MPa, 11.0% ≦ El (B) If 1320 MPa ≦ TS, 9.0% ≦ El × (Fail): (A) If 1180 MPa ≦ TS < 1320 MPa, 11.0% > El (B) If 1320 MPa ≦ TS, 9.0% > El

[0135] ・α 〇 (pass): 80° or more × (fail): less than 80°

[0136] AE 〇 (Pass): The integral value of the load-stroke curve is 70,000 N·mm or more × (Pass): The integral value of the load-stroke curve is less than 70,000 N·mm

[0137] ・Production efficiency E (ton / h) = LS × t × W × ρ × 60 × 10 ―6 Pass (A): 16.0<E<190.0 Pass (B): 3.0<E≦16.0, or 190.0≦E<390.0 Pass (C): 3.0≧E or E≧390.0 Where, LS: sheet threading speed in annealing process (m / min) t: sheet thickness (mm) W: sheet width (mm) ρ: specific gravity of iron (ton / m 3) and ρ=7.86 (ton / m 3 )

[0138] (1) Tensile Test The tensile test was conducted in accordance with JIS Z 2241 (2011). That is, JIS No. 5 test specimens were taken from the obtained steel sheets so that the longitudinal direction was perpendicular to the rolling direction of the base steel sheet. Using the taken test specimens, a tensile test was conducted at a crosshead speed of 10 mm / min, and TS, YS, and El were measured. The results are shown in Table 4.

[0139] (2) VDA Bending Test The VDA bending test was conducted in accordance with the VDA standard (VDA238-100) established by the German Association of the Automotive Industry. Specifically, a 70 mm x 60 mm test piece was obtained from the obtained steel plate by shearing. Here, the 60 mm side was parallel to the rolling (L) direction. The VDA bending test was conducted on the test piece under the following conditions. Test method: Roll support, punch pressing Roll diameter: φ30 mm Punch tip R: 0.4 mm Roll distance: (sheet thickness x 2) + 0.5 mm Stroke speed: 20 mm / min Bending direction: perpendicular to rolling (C) direction At this time, the angle of the outer bend at the center of the plate-shaped test piece when the load F from the pushing bending jig from above is maximum is measured as the bending angle (limit bending angle) (°). In addition, the integral value (absorbed energy) of the load-stroke curve up to the maximum load is calculated using the obtained load-stroke curve. The VDA bending test was carried out three times, and the average values ​​of the limit bending angle at the maximum load and the integral value (absorbed energy) of the load-stroke curve were designated as α (°) and AE, respectively. The results are shown in Table 4.

[0140] In the VDA bending test of steel sheets with a thickness of more than 1.2 mm, the influence of the sheet thickness was taken into consideration, and all tests were performed on steel sheets with a thickness of 1.2 mm. Steel sheets with a thickness of more than 1.2 mm were ground on one side to make the sheet thickness 1.2 mm. Since the grinding process may affect the bendability of the steel sheet surface, the ground surface was set on the inside of the bend (the side that comes into contact with the punch) in the VDA bending test. On the other hand, in the VDA bending test of steel sheets with a thickness of less than 1.2 mm, the influence of the sheet thickness was small, so the test was performed without grinding.

[0141]

[0142]

[0143]

[0144]

[0145]

[0146]

[0147]

[0148] In Tables 1 to 4, underlined values ​​indicate values ​​outside the appropriate range of the present invention. As shown in Table 4, all of the inventive examples were acceptable in terms of tensile strength (TS), yield stress (YS), yield ratio (YR), total elongation (El), limiting bend angle (α) in the VDA bending test, and integral value (absorbed energy) (AE) of the load-stroke curve in the VDA bending test. The production efficiency (E) was also good. On the other hand, in the comparative examples, at least one of tensile strength (TS), yield stress (YS), yield ratio (YR), total elongation (El), limiting bend angle (α) in the VDA bending test, and integral value (absorbed energy) (AE) of the load-stroke curve in the VDA bending test was insufficient.

[0149] Furthermore, the members obtained by forming or joining the steel sheets of the present invention had the excellent properties characteristic of the present invention in all of the tensile strength (TS), yield stress (YS), yield ratio (YR), total elongation (El), limiting bending angle (α) in the VDA bending test, and integral value (absorbed energy) (AE) of the load-stroke curve in the VDA bending test. It was also found that the production efficiency (E) was good.

[0150] F Ferrite BF Bainitic ferrite TM Tempered martensite H Hard second phase L F―MA Length of the ferrite grain boundary in contact with fresh martensite and / or retained austenite

Claims

1. A steel plate having a base steel plate, the base steel plate having a composition containing, in mass%, C: 0.050% or more and 0.400% or less, Si: 0.20% or more and 3.00% or less, Mn: 1.00% or more and less than 3.50%, P: 0.001% or more and 0.100% or less, S: 0.0001% or more and 0.0200% or less, Al: 0.010% or more and 2.000% or less, and N: 0.0100% or less, with the balance being Fe and unavoidable impurities, and a structure at a 1 / 4 position of the plate thickness of the base steel plate having an area ratio of ferrite: less than 20.0% (including 0.0%), an area ratio of retained austenite: 3.0% or more and 15.0% or less, and an area ratio of fresh martensite: 10.0% or less (including 0.0%), The total area ratio of bainitic ferrite and tempered martensite is 45.0% or more and 90.0% or less, and the grain boundary length L of the ferrite grain boundary in contact with fresh martensite and / or retained austenite is F―MA and the grain boundary length L of ferrite F Regarding L F―MA / L F : 0.70 or less, further comprising a surface soft layer formed to a thickness of 20 μm or more from the surface of the base steel sheet in the sheet thickness direction, wherein a total area ratio of structures other than ferrite in the steel structure is ½ or less at a ¼ position in the sheet thickness, and wherein the tensile strength is 1180 MPa or more and less than 1470 MPa.

2. The composition further includes, in mass%, Nb: 0.200% or less, Ti: 0.200% or less, V: 0.200% or less, B: 0.0100% or less, Cr: 1.000% or less, Ni: 1.000% or less, Mo: 1.000% or less, Sb: 0.200% or less, Sn: 0.200% or less, Cu: 1.000% or less, Ta: 0.100% or less, W: 0.500% or less, Mg: 0.0200% or less, Zn: 0.0200% or less, Co: 0.0200% or less, Zr: 0.1000% or less, Ca: 0.0200% or less, Se: 0.0200% or less, The steel plate according to claim 1, containing at least one selected from Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0500% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, and REM: 0.0200% or less.

3. The steel sheet according to claim 1 or 2, which has a zinc-plated layer on one or both sides of the base steel sheet.

4. A member made using the steel plate according to any one of claims 1 to 3.

5. A method for manufacturing a hot-rolled steel sheet by hot rolling a steel slab having the composition according to claim 1 or 2, comprising: a hot rolling process, in which the hot-rolled steel sheet is subjected to pickling; an annealing process, in which the steel sheet after the pickling process is heated and annealed under conditions of an annealing temperature of 720°C to 860°C, a holding time of 20 seconds or more, and a dew point of -10°C or more in an atmosphere; a rapid heating process, in which the steel sheet after the pickling process is rapidly heated from the annealing temperature to the annealing temperature + 10°C or higher under conditions of a heating rate of 10°C / sec or more; a cooling process, in which the steel sheet after the rapid heating process is cooled to a cooling stop temperature of 100°C to 300°C; and a reheating and holding process, in which the steel sheet after the cooling process is heated to a tempering temperature of 460°C or less and held in the temperature range for a tempering time of 10 seconds to 2000 seconds, The method for producing a steel sheet includes a cold rolling step of cold rolling the steel sheet after the pickling step and before the annealing step at a rolling reduction of 20% or more and 80% or less to obtain a cold-rolled steel sheet.

6. The method for producing a steel sheet according to claim 5, wherein the steel sheet passing speed LS (m / min) in the annealing step satisfies the following formula (1): 3.0 / (t×W×4.716×10 ―4 )<LS<390.0 / (t×W×4.716×10 ―4 ) Formula (1) where, t: sheet thickness (mm) after the pickling process and before the annealing process, and W: sheet width (mm) after the pickling process and before the annealing process.

7. A method for producing a steel sheet according to claim 5 or 6, comprising a hot-dip galvanizing step of immersing the steel sheet in a hot-dip galvanizing bath during the cooling step, after the cooling step and before the reheating and holding step, or after the reheating and holding step to form a zinc-plated layer on the steel sheet, or further comprising an alloying treatment step of subjecting the steel sheet on which the zinc-plated layer has been formed to an alloying treatment.

8. The method for producing a steel sheet according to claim 5 or 6, further comprising, after the reheating and holding step, an electrogalvanizing step of immersing the steel sheet in an electrogalvanizing bath to form a zinc-plated layer on the steel sheet.

9. A method for manufacturing a component, comprising the step of subjecting the steel plate according to any one of claims 1 to 3 to at least one of forming and joining to form a component.

Citation Information

Patent Citations

  • High-strength hot-dip galvanized steel sheet with excellent workability and method for manufacturing the same

    JP5256689B2

  • High-strength hot-dip galvanized steel sheet with excellent delayed fracture resistance and method for manufacturing the same

    JP5352793B2

  • High-strength hot-dip galvanized steel sheet with excellent mechanical cutting properties, high-strength alloyed hot-dip galvanized steel sheet, and methods for manufacturing the same.

    JP5354135B2

  • High-strength cold-rolled steel sheet, high-strength galvanized steel sheet, and high-strength alloying hot-dip galvanized steel sheet, excellent in bendability, and method for manufacturing the same

    JP2013163827A

  • High strength hot rolled steel sheet excellent in processability and fatigue characteristic and its manufacturing method

    JP2014173151A