Surface smoothing agent for polyurethane coating film, composition, curing agent, polyurethane resin-forming composition, coating composition, and coating film
The use of a cyclic compound-based surface smoothing agent composition addresses the challenge of achieving high surface smoothness and mechanical properties in polyurethane coatings, resulting in a coating film with improved smoothness and weather resistance.
Patent Information
- Application Number
- PCT/JP2024/008109
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-04
- Publication Date
- 2024-10-03
AI Technical Summary
The increasing demand for high-performance polyurethane coatings has led to a need for new surface smoothing agents that can enhance the smoothness of polyurethane coatings, as existing solutions do not adequately meet the stringent requirements for surface smoothness and mechanical properties.
A surface smoothing agent composition containing a cyclic compound derived from an aliphatic diisocyanate, specifically a polyisocyanate with a cyclic compound represented by formula (1), is used to improve the surface smoothness of polyurethane coatings, which includes a curing agent and a polyurethane resin-forming composition that forms a coating film with excellent smoothness.
The proposed solution achieves a significant improvement in the surface smoothness of polyurethane coatings, with the cyclic compound contributing to enhanced mechanical properties and weather resistance, while maintaining compatibility with polyisocyanate systems.
Smart Images

Figure JP2024008109_03102024_PF_FP_ABST
Abstract
Description
Surface smoothing agent for polyurethane coating film, composition, curing agent, polyurethane resin-forming composition, coating composition and coating film
[0001] The present disclosure relates to a surface-leveling agent for polyurethane coatings, a composition, a curing agent, a polyurethane resin-forming composition, a paint composition, and a coating.
[0002] Known curing agents for forming urethane coating films include those containing derivatives derived from general-purpose aliphatic isocyanates such as hexamethylene diisocyanate, pentamethylene diisocyanate, etc. Polyurethane coating films formed using such curing agents have advantages such as reduced baking temperatures and high weather resistance, and as demand for them increases, the required performance is also becoming higher.
[0003] Here, Patent Document 1 discloses a polyisocyanate composition containing a derivative modified with 1.0 to 5.0 parts by mass of isobutyl alcohol per 100 parts by mass of pentamethylene diisocyanate, and a uretdione derivative consisting of two isocyanate molecules of pentamethylene diisocyanate in a predetermined proportion. According to Patent Document 1, a paint containing a polyurethane resin obtained from this polyisocyanate composition can achieve a good balance between improved hardness, chemical resistance, and surface smoothness.
[0004] Patent No. 6482657
[0005] Journal of Organic Chemistry 1978, 43, 1544-1546 Zhurnal Vsesoyuznogo Khimicheskogo Obshchestva im. D. I. Mendeleeva 1979, 24, 310-311
[0006] However, in recent years in particular, the market has become increasingly demanding in terms of the performance required of polyurethane coating films, and there is a strong demand for the development of new surface smoothing agents for polyurethane coating films that can impart coating film smoothness.
[0007] Therefore, some aspects of the present disclosure are directed to providing a surface-smoothing agent for polyurethane coating films, a composition, a curing agent, a polyurethane resin-forming composition, and a coating composition that contribute to the production of coating films with excellent surface smoothness. Another aspect of the present disclosure is directed to providing a coating film with excellent surface smoothness.
[0008] In some aspects, the present disclosure provides the following [1] to
[10] .
[0009] [1] A composition containing a polyisocyanate, wherein the polyisocyanate contains a derivative derived from an aliphatic diisocyanate, and the content of a cyclic compound represented by the following formula (1) is 0.1 to 15 mass % relative to the total amount of the composition: [In formula (1), n is an integer of 1 to 6, and R 1 and R 2 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.
[0010] [2] The composition according to [1], wherein the derivative includes an isocyanurate derived from an aliphatic diisocyanate.
[0011] [3] The composition according to [1] or [2], wherein the aliphatic diisocyanate includes butane diisocyanate.
[0012] [4] The R 1 and the R 2 are each independently a hydrogen atom, an aliphatic group having 1 to 20 carbon atoms, an alicyclic group having 3 to 20 carbon atoms, or an aromatic group having 6 to 20 carbon atoms, and the aliphatic group, the alicyclic group, and the aromatic group may be substituted with a substituent, and may contain one or more atoms selected from the group consisting of an oxygen atom, a nitrogen atom, and a sulfur atom.
[0013] [5] The R 1 and the R 2 [5] The composition according to any one of [1] to [4], wherein one of the groups is a hydrogen atom and the other is a monovalent organic group having 1 to 20 carbon atoms.
[0014] [6] A curing agent for forming a polyurethane resin, comprising the composition according to any one of [1] to [5].
[0015] [7] A polyurethane resin-forming composition comprising the composition according to any one of [1] to [5] and a polyol.
[0016] [8] A coating composition comprising the polyurethane resin-forming composition according to [7].
[0017] [9] A coating film comprising a cured product of the coating composition according to [8].
[0018]
[10] A surface smoothing agent for polyurethane coating films, comprising a cyclic compound represented by the following formula (1):
[0019] [In formula (1), n is an integer of 1 to 6, and R 1 and R 2 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.
[0020] According to some aspects of the present disclosure, it is possible to provide a surface-smoothing agent for polyurethane coating films, a composition, a curing agent, a polyurethane resin-forming composition, and a paint composition, which contribute to the production of coating films with excellent surface smoothness. According to another aspect of the present disclosure, it is possible to provide a coating film with excellent surface smoothness.
[0021] In this specification, a numerical range indicated using "to" indicates a range that includes the numerical values written before and after "to" as the minimum and maximum values, respectively. Furthermore, unless specifically stated otherwise, the units of the numerical values written before and after "to" are the same. In the numerical ranges described in stages in this specification, the upper limit or lower limit of a numerical range in a certain stage may be replaced with the upper limit or lower limit of a numerical range in another stage. Furthermore, in the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in the examples. Furthermore, the upper limit and lower limit values individually described can be combined in any way. Furthermore, in this specification, "(meth)acrylic" means at least one of acrylic and the corresponding acrylic.
[0022] Preferred embodiments of each aspect of the present disclosure will be described below, although the aspects of the present disclosure are not limited to the following embodiments.
[0023] <Surface-leveling agent for polyurethane coating films> A surface-leveling agent for polyurethane coating films according to one embodiment of the present disclosure contains a cyclic compound represented by formula (1) (hereinafter referred to as "cyclic compound A").
[0024]
[0025] In formula (1), n is an integer of 1 to 6. Therefore, cyclic compound A can be said to be a compound having a cyclic urea group of 5 to 10 members in the molecule. 1 and R 2 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.
[0026] The cyclic compound A can improve the surface smoothness of the polyurethane coating film.
[0027] From the viewpoints of feasibility on an industrial scale and improving compatibility with polyisocyanate, n in formula (1) may be an integer of 1 to 4. That is, cyclic compound A may be a compound having a cyclic urea group having a 5- to 8-membered ring.
[0028] R in formula (1) 1 and R 2 From the viewpoint of improving the mechanical properties of the coating film, one of the groups may be a hydrogen atom and the other may be a monovalent organic group having 1 to 20 carbon atoms.
[0029] The monovalent organic group may have 3 to 18 carbon atoms, or may have 6 to 17 carbon atoms.
[0030] From the viewpoint of improving compatibility with polyisocyanate and suppressing deterioration in the physical properties of the coating film, the monovalent organic group may be an aliphatic group having 1 to 20 carbon atoms, an alicyclic group having 3 to 20 carbon atoms, or an aromatic group having 6 to 20 carbon atoms. These groups may be substituted with a substituent and may contain one or more atoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms. In other words, the aliphatic group, alicyclic group, and aromatic group in this specification include groups composed only of carbon atoms and hydrogen atoms, as well as groups in which a portion of the group is substituted with a substituent and / or one or more atoms selected from the group consisting of oxygen atoms, nitrogen atoms, and sulfur atoms.
[0031] The number of substituents may be, for example, 1 to 5. Examples of the substituent include a hydroxy group, an alkoxy group, an amino group, an amide group, a carboxy group, a carbonyl group, an ester group, an ether group, a thiol group, a thioether group, a vinyl group, an aryl group, an isocyanate group, and a halogeno group. In particular, when the monovalent organic group is substituted with an isocyanate group, that is, when the cyclic compound A is an isocyanate compound, the cyclic compound A is chemically bonded to the polyurethane coating film, thereby preventing the cyclic compound A from being liberated. The number of isocyanate groups possessed by the cyclic compound may be 2 or more, but from the viewpoint of improving the coating film smoothness, it is 1.
[0032] The aliphatic group having 1 to 20 carbon atoms may be linear or branched. Examples of the aliphatic group having 1 to 20 carbon atoms include alkyl groups, alkoxy groups, alkenyl groups, hydroxyalkyl groups, hydroxyalkoxy groups, alkyl groups substituted with an alkoxy group, haloalkyl groups, dihaloalkyl groups, trihaloalkyl groups, alkylamino groups, aminoalkyl groups, alkoxycarbonyl groups, alkylcarbonyl groups, monoalkylamide groups and alkylamide groups which may be substituted with an isocyanate group. The carbon chain of these groups may be linear or branched.
[0033] Examples of the alicyclic group having 3 to 20 carbon atoms include a cycloalkyl group and a bicycloalkyl group.
[0034] Examples of the aromatic group having 6 to 20 carbon atoms include a phenyl group, an alkoxyphenyl group, an arylamino group, a diarylamino group, an arylalkylamino group, a cyclic amino group, an arylcarbonyl group, and an aroyl group.
[0035] From the viewpoint of improving the mechanical properties of the coating film, the monovalent organic group may be a group represented by the following formula (i).
[0036] In formula (i), X is CH or N, and R 3 and R 4 are each independently a hydrogen atom or a monovalent organic group having 1 to 18 carbon atoms, and * is a bond bonded to N in formula (1). X may be N from the viewpoint of further improving the mechanical properties of the coating film. Examples of monovalent organic groups are the same as the examples of monovalent organic groups described above, except for the number of carbon atoms. For example, R 3 and R 4 From the viewpoint of compatibility with polyisocyanate, R may be an aliphatic group having 1 to 18 carbon atoms, an alicyclic group having 3 to 18 carbon atoms, or an aromatic group having 6 to 18 carbon atoms. 3 and R 4 R may be a monovalent organic group substituted with an isocyanate group from the viewpoint of preventing the cyclic compound from being released from the coating film. 3 and R 4 From the viewpoint of further improving the mechanical properties of the coating film while maintaining good compatibility with the polyisocyanate, one of the groups may be a hydrogen atom and the other may be a monovalent organic group having 1 to 18 carbon atoms.
[0037] From the viewpoint of improving compatibility with polyisocyanate and preventing separation from the coating film, the cyclic compound A may be a compound represented by the following formula (1A).
[0038] In formula (1A), m may be an integer of 1 to 4.
[0039] Specific examples of the cyclic compound A include compounds represented by the following formulas (2) to (4).
[0040] The cyclic compound A can be synthesized, for example, in accordance with the synthesis methods described in Non-Patent Documents 1 and 2, the synthesis methods described in the Examples described later, and the like. Alternatively, the cyclic compound A can be obtained by carrying out an isocyanuration reaction of an aliphatic diisocyanate in a diluted state with an organic solvent, thereby allowing the reaction to produce the cyclic compound A to proceed. Hereinafter, the reaction to produce the cyclic compound A is referred to as a cyclization reaction. Details of the isocyanuration will be described later.
[0041] The cyclic compound A may be the main component of the surface-smoothing agent for polyurethane coatings. The surface-smoothing agent for polyurethane coatings may consist solely of the cyclic compound A, or may contain components other than the cyclic compound A (such as components mixed in during the production of the cyclic compound A). The content of the cyclic compound A may be, for example, 60% by mass or more, 80% by mass or more, or 90% by mass or more, based on the total mass of the surface-smoothing agent for polyurethane coatings.
[0042] <Composition> A composition according to one aspect of the present disclosure is a composition containing a polyisocyanate (hereinafter also referred to as a "polyisocyanate composition"), in which the polyisocyanate contains a derivative (hereinafter also referred to as a "derivative A") derived from an aliphatic diisocyanate, and the content of the cyclic compound A described above is 0.1 to 15 mass % with respect to the total amount of the composition (polyisocyanate composition).
[0043] The composition can be used as a curing agent for forming a polyurethane resin, and the composition can provide a curing agent that contributes to the formation of a polyurethane coating film with excellent surface smoothness.
[0044] The aliphatic diisocyanate may be, for example, a diisocyanate represented by the formula OCN-R-NCO (R is an alkylene group having 2 to 30 carbon atoms which may be substituted with a substituent). The alkylene group may have 2 to 4 carbon atoms. Examples of the substituent include an alkyl group, a carbonyl group, an ester group, a vinyl group, an aryl group, an ether group, a thioether group, and a halogeno group.
[0045] Specific examples of aliphatic diisocyanates include ethane diisocyanate, propane diisocyanate, butane diisocyanate, hexamethylene diisocyanate, lysine diisocyanate, etc. Among these, when butane diisocyanate is used (i.e., when the polyisocyanate composition contains a derivative derived from an aliphatic diisocyanate including butane diisocyanate), compatibility with cyclic compound A is good and the coating film tends to have higher hardness.
[0046] The aliphatic diisocyanates may be used singly or in combination of two or more. In other words, the derivative A may be rephrased as a derivative derived from at least one aliphatic diisocyanate.
[0047] Derivative A may be an isocyanurate, iminooxadiazinedione, oxadiazinetrione, uretdione, allophanate, biuret, or adduct with a compound having a hydroxyl group. In particular, when an isocyanurate is used as derivative A (i.e., when the polyisocyanate composition contains an isocyanurate derived from an aliphatic diisocyanate), the weather resistance and hardness of the resulting coating film tend to be improved. The isocyanurate may be a mononuclear isocyanurate (an aliphatic diisocyanate trimer having one isocyanurate group) or a polynuclear isocyanurate, or a mixture thereof.
[0048] The content of the isocyanurate mononuclear compound may be 40% by mass or more, 50% by mass or more, or 60% by mass or more, relative to the total amount of the polyisocyanate composition, from the viewpoint of improving the weather resistance and hardness of the resulting coating film. The content of the isocyanurate mononuclear compound may be 85% by mass or less, 75% by mass or less, or 65% by mass or less, relative to the total amount of the polyisocyanate composition, from the viewpoint of improving the application properties of the resulting coating film. From the above viewpoint, the content of the isocyanurate mononuclear compound may be 40 to 85% by mass, relative to the total amount of the polyisocyanate composition.
[0049] The content of the isocyanurate mononuclear compound can be measured, for example, by gel permeation chromatography (GPC). More specifically, it can be measured in accordance with the examples described below.
[0050] The content of derivative A may be 80 to 99.9% by mass, relative to the total amount of the polyisocyanate composition, from the viewpoint of making it easier to obtain a cured film having superior surface smoothness. From the same viewpoint, the content of derivative A may be 85% by mass or more, 90% by mass or more, 92% by mass or more, or 95% by mass or more, relative to the total amount of the polyisocyanate composition, and may be 99% by mass or less, or 98% by mass or less. Note that, when cyclic compound A is a derivative derived from an aliphatic diisocyanate, the above "content of derivative A" does not include the content of cyclic compound A. The same applies to the content of derivative A in the "total amount of the content of derivative A and the content of cyclic compound A" described below.
[0051] The cyclic compound A is a compound represented by the above formula (1). Details of the cyclic compound A are omitted because they are the same as those of the cyclic compound A contained in the surface smoothing agent for polyurethane coatings.
[0052] From the viewpoint of making it easier to obtain a cured film having better surface smoothness, the content of cyclic compound A may be 1% by mass or more, or 2% by mass or more, and may be 10% by mass or less, 8% by mass or less, or 5% by mass or less, relative to the total amount of the polyisocyanate composition.
[0053] In this embodiment, the content of cyclic compound A relative to the total content of derivative A and cyclic compound A may be 0.1 to 15% by mass. The content may be 1% by mass or more, or 2% by mass or more, or may be 10% by mass or less, 8% by mass or less, or 5% by mass or less.
[0054] The content of cyclic compound A can be measured, for example, by gel permeation chromatography (GPC). More specifically, it can be measured in accordance with the examples described below.
[0055] The polyisocyanate composition may contain components other than the above-mentioned compounds (components mixed in during the production of derivative A, components mixed in during the production of cyclic compound A, etc.) to the extent that the effects of the present disclosure are not impaired.
[0056] The polyisocyanate composition may be obtained by mixing a previously synthesized derivative A with a cyclic compound A. For example, the polyisocyanate composition can be prepared by adding the cyclic compound A to a composition containing a polyisocyanate obtained by isocyanating an aliphatic diisocyanate. Alternatively, as described above, the polyisocyanate composition can also be obtained by carrying out the isocyanuration reaction of an aliphatic diisocyanate in a diluted state with an organic solvent.
[0057] A commonly known isocyanuration catalyst can be used for isocyanuration to form isocyanurate groups. Examples of isocyanuration catalysts for aliphatic diisocyanates include quaternary onium salts, metal carboxylate salts, and aminosilyl group-containing compounds. These isocyanuration catalysts can be used alone or in combination of two or more.
[0058] The isocyanuration catalyst may be an aminosilyl group-containing compound such as aminosilane or silyl urea, from the viewpoint of suppressing the formation of high molecular weight compounds. In particular, when a disilazane such as hexamethyldisilazane or heptamethyldisilazane is used, the formation of high molecular weight compounds can be further suppressed.
[0059] The amount of these catalysts used varies depending on the type of catalyst used, but may be 0.01 to 10% by mass, or may be 0.1 to 3% by mass, based on the amount of the isocyanate compound charged.
[0060] The reaction temperature for isocyanuration may be 60 to 180° C., or may be 100 to 160° C. When the reaction temperature for isocyanuration is 60° C. or higher, the reaction time can be shortened, and coloration of the polyisocyanate composition can be further suppressed.
[0061] During isocyanuration, a reaction terminator may be added to terminate the reaction when the target isocyanate group content and molecular weight are reached. The reaction terminator has the effect of deactivating the catalyst, and specific examples thereof include water and compounds having a hydroxyl group. Alcohols may also be used as the reaction terminator. These terminators may be used alone or in combination of two or more. It is preferable to add the reaction terminator promptly after the target isocyanate group content and molecular weight are reached.
[0062] The amount of reaction terminator added varies depending on the type of reaction terminator and the type of catalyst used, but may be 0.1 to 3.5 equivalents or 0.8 to 2.5 equivalents of the catalyst. When the reaction terminator is 0.1 equivalent or more, the storage stability of the resulting polyisocyanate composition is further improved. When the reaction terminator is 3.5 equivalents or less, the generation of a reaction product between the reaction terminator and the aliphatic diisocyanate can be further suppressed, and therefore, a decrease in the isocyanate group content can be more effectively suppressed.
[0063] When a cyclization reaction is carried out (i.e., when a reaction to produce cyclic compound A is carried out by carrying out an isocyanuration reaction of an aliphatic diisocyanate in a diluted state with an organic solvent), the cyclization reaction is facilitated by using an aliphatic diisocyanate having 4 or less carbon atoms. In particular, the use of butane diisocyanate provides a good balance between the reaction rates of the cyclization reaction and the isocyanuration reaction.
[0064] When carrying out a cyclization reaction, an organic solvent having a boiling point equal to or higher than the reaction temperature may be used, as long as it does not affect the reaction. Examples of organic solvents include aliphatic hydrocarbons such as octane, alicyclic hydrocarbons such as cyclohexane and methylcyclohexane, ketones such as methyl isobutyl ketone and cyclohexanone, esters such as butyl acetate and isobutyl acetate, glycol ether esters such as ethylene glycol ethyl ether acetate, propylene glycol monomethyl ether acetate, 3-methyl-3-methoxybutyl acetate, and ethyl-3-ethoxypropionate, ethers such as dioxane, halogenated hydrocarbons such as methylene iodide and monochlorobenzene, and polar aprotic solvents such as N-methylpyrrolidone, dimethylformamide, dimethylacetamide, dimethyl sulfoxide, and hexamethylphosphonylamide. These solvents may be used alone or in combination of two or more.
[0065] The substrate concentration may be 20 to 80% by mass, 30 to 70% by mass, or 40 to 60% by mass. If the substrate concentration is within the above range, the cyclization reaction time can be shortened, and therefore coloration and viscosity increase of the product can be further suppressed.
[0066] The cyclization reaction time varies depending on the type of catalyst used, the amount of catalyst added, the substrate concentration, the reaction temperature, etc., but may be 150 minutes or less, 140 minutes or less, or 120 minutes or less. By setting the cyclization reaction time to 150 minutes or less, the amount of cyclic compound A produced can be easily controlled to 15 mass% or less.
[0067] The isocyanuration reaction and the cyclization reaction can be carried out sequentially or in parallel. By diluting the reaction system with an organic solvent during or after the isocyanuration reaction and then carrying out the cyclization reaction, coloration of the reaction solution and thickening of the product can be suppressed.
[0068] The organic solvent used in the reaction may be removed simultaneously with the removal of the free aliphatic diisocyanate. To remove the free aliphatic diisocyanate, for example, a removal method using thin film distillation at 90 to 140°C under a high vacuum of 10 to 300 Pa or an extraction method using an organic solvent may be applied. The residual content of the free aliphatic diisocyanate present in the reaction solution may be 5% by mass or less. When the residual content of the aliphatic diisocyanate is 5% by mass or less, odor generation can be further suppressed and a decrease in storage stability can be suppressed.
[0069] For the purpose of extending the pot life, making the coating composition one-component, etc., the polyisocyanate in the polyisocyanate composition may be converted into a blocked isocyanate using a known blocking agent. That is, the polyisocyanate in the polyisocyanate composition may be a blocked isocyanate. Blocked isocyanates are inactive at room temperature, but when heated, the blocking agent dissociates and the isocyanate group is activated again, thereby imparting a latent function of reacting with active hydrogen groups.
[0070] The blocking agent is a compound having one active hydrogen atom in the molecule, and examples thereof include alcohol-based, alkylphenol-based, phenol-based, active methylene, mercaptan-based, acid amide-based, acid imide-based, imidazole-based, urea-based, oxime-based, amine-based, imide-based, and pyrazole-based compounds.
[0071] The polyisocyanate composition described above may be used alone or in combination with other components as a curing agent.
[0072] <Curing Agent> A curing agent according to one embodiment of the present disclosure is a curing agent for forming a polyurethane resin, which contains the composition (polyisocyanate composition) according to the above embodiment.
[0073] The above curing agent makes it possible to form a polyurethane coating film with excellent surface smoothness.
[0074] The curing agent may consist solely of the polyisocyanate composition, or may contain components other than the polyisocyanate composition, such as additives that can be contained in the coating composition described below.
[0075] The content of cyclic compound A in the curing agent may be 0.1 to 15% by mass, 1% by mass or more, or 2% by mass or more, or 10% by mass or less, 8% by mass or less, or 5% by mass or less, based on the total content of derivative A and cyclic compound A.
[0076] <Polyurethane Resin-Forming Composition> A polyurethane resin-forming composition according to one embodiment of the present disclosure includes the polyisocyanate composition of the above embodiment and a polyol. The polyurethane resin-forming composition may also be a composition including the curing agent of the above embodiment and a polyol.
[0077] The polyurethane resin-forming composition can be used in a coating material for forming a coating film. The polyurethane resin-forming composition can provide a coating material composition capable of forming a polyurethane coating film having excellent surface smoothness.
[0078] The polyurethane resin-forming composition may be a one-component composition in which all of the constituent components are contained in one component, or a multi-component composition in which the constituent components are present in multiple components. For example, the polyurethane resin-forming composition may contain a first component (main component) containing a polyol and a second component (curing agent) containing a polyisocyanate composition. The polyurethane resin-forming composition may contain the first component, the second component, and a third component other than these. When the polyurethane resin-forming composition is a multi-component composition, the other constituent components (catalyst, etc.) may be contained in the first component, the second component, or the third component.
[0079] The polyol is a compound containing an active hydrogen group as a reactive group with an isocyanate group. The polyol is not particularly limited, and examples thereof include polyester polyol, polyether polyol, polycarbonate polyol, polyolefin polyol, acrylic polyol, silicone polyol, castor oil-based polyol, fluorine-based polyol, transesterification products of two or more polyols, and hydroxyl-terminated prepolymers obtained by urethane reaction with polyisocyanate. These may be used alone or in combination of two or more.
[0080] (Polyester Polyol) Examples of polyester polyols include those obtained by a condensation polymerization reaction between one or more dicarboxylic acids or anhydrides thereof and one or more low-molecular-weight polyols having a molecular weight of not more than 500. Examples of dicarboxylic acids include phthalic acid, isophthalic acid, terephthalic acid, naphthalenedicarboxylic acid, succinic acid, tartaric acid, oxalic acid, malonic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, glutaconic acid, azelaic acid, sebacic acid, 1,4-cyclohexyldicarboxylic acid, α-hydromuconic acid, β-hydromuconic acid, α-butyl-α-ethylglutaric acid, α,β-diethylsuccinic acid, maleic acid, and fumaric acid. Examples of low molecular weight polyols having a molecular weight of 500 or less include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 3-methyl-1,5-pentanediol, 3,3-dimethylolheptane, diethylene glycol, dipropylene glycol, neopentyl glycol, cyclohexane-1,4-diol, cyclohexane-1,4-dimethanol, dimer diol, bisphenol A, ethylene oxide or propylene oxide adducts of bisphenol A, bis(β-hydroxyethyl)benzene, xylylene glycol, glycerin, trimethylolpropane, and pentaerythritol. Also usable are lactone-based polyester polyols obtained by ring-opening polymerization of cyclic ester (so-called lactone) monomers such as ε-caprolactone, alkyl-substituted ε-caprolactone, δ-valerolactone, alkyl-substituted δ-valerolactone, etc. Furthermore, it is also possible to use polyester-amide polyols obtained by replacing a portion of the low-molecular-weight polyol with a low-molecular-weight polyamine or low-molecular-weight amino alcohol such as hexamethylenediamine, isophoronediamine, or monoethanolamine.
[0081] (Polyether Polyol) Examples of polyether polyols include polyether polyols obtained by addition polymerization of alkylene oxides using a compound having two or more (e.g., 2 to 3) active hydrogen groups as an initiator, such as low molecular weight polyols and low molecular weight polyamines. Examples of low molecular weight polyols include the same compounds exemplified as the low molecular weight polyols having a molecular weight of 500 or less. Examples of low molecular weight polyamines include ethylene diamine, propylene diamine, toluene diamine, metaphenylenediamine, diphenylmethane diamine, and xylylene diamine. Examples of alkylene oxides include ethylene oxide, propylene oxide, and butylene oxide. In addition, polyether polyols obtained by ring-opening polymerization of alkyl glycidyl ethers such as methyl glycidyl ether, aryl glycidyl ethers such as phenyl glycidyl ether, and cyclic ether monomers such as tetrahydrofuran can also be used.
[0082] (Polycarbonate polyol) Examples of polycarbonate polyols include those obtained by the dealcoholization or dephenolation reaction of one or more low molecular weight polyols with diaryl carbonates. Examples of low molecular weight polyols include the same compounds as those exemplified as low molecular weight polyols having a molecular weight of 500 or less. Examples of diaryl carbonates include dialkyl carbonates such as dimethyl carbonate and diethyl carbonate, alkylene carbonates such as ethylene carbonate and propylene carbonate, diphenyl carbonate, dinaphthyl carbonate, dianthryl carbonate, diphenanthryl carbonate, diindanyl carbonate, and tetrahydronaphthyl carbonate. In addition, examples of polycarbonate polyols include polyols obtained by transesterification of polycarbonate polyol, polyester polyol, and low molecular weight polyol.
[0083] (Polyolefin Polyol) Examples of polyolefin polyols include polybutadiene having two or more hydroxyl groups, hydrogenated polybutadiene, polyisoprene, and hydrogenated polyisoprene.
[0084] (Acrylic Polyol) Examples of acrylic polyols include those obtained by polymerizing or copolymerizing an acrylic acid ester and / or a methacrylic acid ester (hereinafter referred to as a (meth)acrylic acid ester), an acrylic acid hydroxy compound and / or a methacrylic acid hydroxy compound (hereinafter referred to as a (meth)acrylic acid hydroxy compound), and a polymerization initiator using light energy such as ultraviolet light or an electron beam, or heat energy.
[0085] ((Meth)acrylic acid esters) Examples of (meth)acrylic acid esters include alkyl esters having 1 to 20 carbon atoms. Examples of such (meth)acrylic acid esters include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, and dodecyl (meth)acrylate; esters of (meth)acrylic acid with alicyclic alcohols such as cyclohexyl (meth)acrylate; and (meth)acrylic acid aryl esters such as phenyl (meth)acrylate and benzyl (meth)acrylate. These (meth)acrylic acid esters can be used alone or in combination of two or more.
[0086] ((Meth)acrylic Acid Hydroxy Compound) The (meth)acrylic acid hydroxy compound has at least one hydroxyl group in the molecule that can serve as a reaction site with polyisocyanate. Examples of the (meth)acrylic acid hydroxy compound include acrylic acid hydroxy compounds such as 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 3-hydroxy-2,2-dimethylpropyl acrylate, and pentaerythritol triacrylate. Methacrylic acid hydroxy compounds such as 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 4-hydroxybutyl methacrylate, 3-hydroxy-2,2-dimethylpropyl methacrylate, and pentaerythritol trimethacrylate can also be used. The (meth)acrylic acid hydroxy compound can be used alone or in combination of two or more.
[0087] (Silicone Polyol) Examples of silicone polyols include vinyl group-containing silicone compounds obtained by polymerizing γ-methacryloxypropyltrimethoxysilane, and polysiloxanes having at least one terminal hydroxyl group in the molecule, such as α,ω-dihydroxypolydimethylsiloxane and α,ω-dihydroxypolydiphenylsiloxane.
[0088] (Castor oil-based polyol) Examples of the castor oil-based polyol include linear or branched polyester polyols obtained by reacting castor oil fatty acids with polyols. In addition, dehydrated castor oil, partially dehydrated castor oil, and hydrogenated castor oil can also be used.
[0089] (Fluorine-Based Polyol) Examples of fluorine-based polyols include linear or branched polyols obtained by copolymerization of a fluorine-containing monomer and a monomer having a hydroxy group as an essential component. Here, the fluorine-containing monomer may be a fluoroolefin. Examples of fluorine-containing monomers include tetrafluoroethylene, chlorotrifluoroethylene, trichlorofluoroethylene, hexafluoropropylene, vinylidene fluoride, vinyl fluoride, trifluoromethyltrifluoroethylene, and the like. Furthermore, examples of monomers having a hydroxyl group include hydroxyalkyl vinyl ethers such as hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, and cyclohexanediol monovinyl ether; hydroxyalkyl allyl ethers such as 2-hydroxyethyl allyl ether; hydroxyl group-containing vinyl carboxylates such as hydroxyalkyl vinyl crotonate; and hydroxy group-containing allyl esters.
[0090] The number of active hydrogen groups (average number of functional groups) in one molecule of the polyol may be 1.9 to 6.0. If the number of active hydrogen groups is within the above range, the resulting coating film will exhibit excellent hardness.
[0091] The number average molecular weight of the polyol may be in the range of 750 to 50000. When the number average molecular weight of the polyol is 750 or more, the adhesion is further improved, and when it is 50000 or less, the solubility in low-polarity organic solvents is further improved, and the adhesion is further improved.
[0092] The content ratio of the polyisocyanate composition to the polyol in the polyurethane resin-forming composition is not particularly limited, but the molar ratio of the isocyanate groups in the polyisocyanate composition to the hydroxyl groups in the polyol (R = isocyanate groups / hydroxyl groups) may be 0.5 to 2.5. When the molar ratio is 0.5 or more, the hydroxyl groups do not become too excessive, further improving adhesion. In addition, a decrease in crosslink density is suppressed, and the durability and mechanical strength of the coating film become even better. When the molar ratio is 2.5 or less, the isocyanate groups do not become too excessive, suppressing reaction with moisture in the air, further reducing swelling of the coating film and further suppressing the associated decrease in adhesion. From the same viewpoint as above, the ratio of the total number of moles of isocyanate groups contained in the isocyanate group-containing compound contained in the polyurethane resin-forming composition to the total number of moles of hydroxyl groups contained in the hydroxyl group-containing compound contained in the polyurethane resin-forming composition (R' = isocyanate groups / hydroxyl groups) may be 0.5 to 2.5.
[0093] The organic solvent used as the dilution solvent can be appropriately selected from the group consisting of ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, etc., esters such as ethyl acetate, butyl acetate, cellosolve acetate, etc., alcohols such as butanol, isopropyl alcohol, etc., hydrocarbons such as toluene, xylene, cyclohexane, mineral spirits, naphtha, etc., depending on the purpose and application. These solvents may be used alone or in combination of two or more.
[0094] <Coating Composition> A coating composition according to one embodiment of the present disclosure includes the polyurethane resin-forming composition of the above embodiment.
[0095] The coating composition may contain a known urethanization catalyst as appropriate, taking into consideration pot life, curing conditions, working conditions, etc. Examples of urethanization catalysts include organometallic compounds such as dibutyltin diacetate, dibutyltin dilaurate, and dioctyltin dilaurate, and organic amines such as triethylenediamine and triethylamine, and salts thereof. These catalysts may be used alone or in combination of two or more.
[0096] The curing conditions for the coating composition are not particularly limited, but the curing temperature may be −5 to 150° C., the humidity may be 10 to 95% RH, and the curing time may be 0.5 to 336 hours.
[0097] The coating composition may contain additives such as antioxidants such as 2,6-di-tert-butyl-4-methylphenol, ultraviolet absorbers, pigments, dyes, solvents, flame retardants, hydrolysis inhibitors, lubricants, plasticizers, fillers, antistatic agents, dispersants, catalysts, storage stabilizers, surfactants, and leveling agents, as needed.
[0098] <Coating Film (Cured Film)> A coating film according to one embodiment of the present disclosure comprises a cured product of the coating composition of the above embodiment.
[0099] The coating film is formed using the coating composition of the above embodiment. Therefore, the coating film has excellent surface smoothness. The excellent surface smoothness of the coating film can be confirmed, for example, by the arithmetic mean roughness of the coating film at 23°C. The arithmetic mean roughness of the coating film can be measured in accordance with JIS B0601. The arithmetic mean roughness of the coating film at 23°C is, for example, 150 nm or less, and may be 125 nm or less, or 100 nm or less.
[0100] The coating film can be formed by applying the coating composition onto the surface of the substrate by a known method such as spraying, brushing, dipping, or using a coater, and then curing the composition.
[0101] The adherend is not particularly limited, and examples thereof include stainless steel, phosphate-treated steel, zinc steel, iron, copper, aluminum, brass, glass, slate, acrylic resin, polycarbonate resin, polyethylene terephthalate resin, polyethylene naphthalate resin, polybutylene phthalate resin, polystyrene resin, AS resin, ABS resin, polycarbonate-ABS resin, 6-nylon resin, 6,6-nylon resin, MXD6 nylon resin, polyvinyl chloride resin, polyvinyl alcohol resin, polyurethane resin, phenolic resin, melamine resin, polyacetal resin, chlorinated polyolefin resin, polyolefin resin, polyamide resin, polyether ether ketone resin, polyphenylene sulfide resin, NBR resin, chloroprene resin, SBR resin, and SEBS resin. Adherends molded from materials such as polyethylene and polypropylene that have been subjected to corona discharge treatment or other surface treatments, and adherends having a coating layer formed on the surface of the adherend that can serve as an intermediate can be used.
[0102] The thickness of the coating film formed on the surface layer of the adherend may be 10 μm or more from the viewpoint of obtaining a coating film that is excellent in recoatability, durability, etc. When the film thickness is 10 μm or more, durability is improved and the occurrence of breakage of the coating film due to impact can be further suppressed.
[0103] The present disclosure will be described in more detail below using examples and comparative examples, but the present disclosure is not limited to the following examples.
[0104] First, specific synthesis examples for producing a compound having a cyclic urea group (cyclic compound A) contained in the polyisocyanate composition of the present embodiment will be described, but the cyclic compound contained in the polyisocyanate composition according to one aspect of the present disclosure is not limited to these.
[0105] Synthesis Example 1: 1.0 g of 1,3-diazocan-2-one and 1.2 g of triethylamine were charged into a 100 mL four-neck flask equipped with a stirrer, thermometer, condenser, and nitrogen gas inlet tube, and dissolved in 41 g of methylene chloride. This was heated to 80°C, and 1.3 g of 2-ethylhexanoyl chloride was slowly added dropwise over 20 minutes, followed by stirring for 60 minutes. The reaction solution was then cooled to room temperature, and the precipitated hydrochloride was removed by filtration. The methylene chloride in the filtrate was distilled off under reduced pressure using an evaporator. 20 g of water was added to the concentrate, and the mixture was stirred vigorously. The precipitate was then collected by filtration and washed with 5.0 g of water, yielding 1.5 g of cyclic compound Cy-1. Cy-1 is represented by the following formula (2):
[0106]
[0107] Synthesis Example 2: 1.0 g of 1,2-diisocyanatoethane and 4.0 g of ethyl acetate were placed in a 50 mL three-necked flask equipped with a stirrer and a nitrogen gas inlet tube, and the mixture was heated to 40°C. 2.2 g of dioctylamine was slowly added dropwise over 10 minutes, and the mixture was stirred for 30 minutes. The ethyl acetate was then removed under reduced pressure using an evaporator, yielding 3.2 g of cyclic compound Cy-2. Cy-2 is represented by the following formula (3):
[0108]
[0109] Example 1 Synthesis of Polyisocyanate Composition 500 g of 1,4-butane diisocyanate (NCO content: 60.0% by mass, hereinafter abbreviated as BDI) was charged into a 1 L four-neck flask equipped with a stirrer, thermometer, condenser, and nitrogen gas inlet tube, and the mixture was heated to 100°C. 5.0 g of hexamethyldisilazane, an isocyanuration catalyst, was added, and the mixture was heated to 120°C and stirred for 1.7 hours. Thereafter, 500 g of butyl acetate was added and stirred for 15 minutes. Thereafter, the mixture was cooled to 50°C in a water bath, and 3.0 g of ethanol, a reaction terminator, was added, and the termination reaction was carried out at 50°C for 30 minutes. After cooling the reaction solution, excess BDI and butyl acetate were removed by thin-film distillation (conditions: 110°C, 0.04 kPa), yielding 62 g of polyisocyanate composition P-1. P-1 contained 1.6% by mass of a compound represented by the following formula (4) (cyclic compound Cy-3) and 59.0% by mass of an isocyanurate mononuclear product. In this example, the cyclic compound content and the isocyanurate mononuclear product content were measured by the following methods.
[0110]
[0111] (Measurement of cyclic compound content and isocyanurate mononuclear content) The cyclic compound content and isocyanurate mononuclear content relative to the total amount of the polyisocyanate composition were measured by GPC using the following apparatus: Apparatus: HLC-8420 (manufactured by Tosoh Corporation) Column: TSKgel (manufactured by Tosoh Corporation) G3000H-XL, G2000H-XL, G1000H-XL, one each connected in series Carrier: Tetrahydrofuran Detection method: Differential refractive index detector
[0112] The differential refractive index peak of a cyclic compound varies depending on the chemical structure of the cyclic compound, but in the case of Cy-3 (compound of formula (4)), it appears at a retention time of approximately 25.9 minutes. The area of this peak was determined, and the content of the cyclic compound was calculated using the following formula: Content of cyclic compound (mass%) = Peak area at retention time 25.9 minutes / Total area of all peaks × 100 The retention times of Cy-1 and Cy-2 are approximately 25.1 minutes and approximately 26.4 minutes, respectively.
[0113] The differential refractive index peak of the isocyanurate mononuclear compound differs depending on the type of aliphatic diisocyanate used, but when 1,4-butane diisocyanate is used, it appears at a retention time of approximately 23.8 minutes. The area of this peak was determined, and the content of the isocyanurate mononuclear compound was calculated using the following formula: Content (mass%) of isocyanurate mononuclear compound = Peak area at retention time 23.8 minutes / Total area of all peaks × 100
[0114] Example 2: 500 g of BDI was charged into a 1 L four-neck flask equipped with a stirrer, thermometer, condenser, and nitrogen gas inlet tube. The mixture was heated to 100°C, and 5.0 g of hexamethyldisilazane, an isocyanurate catalyst, was added. The mixture was then heated to 120°C and stirred for 1.7 hours. 500 g of butyl acetate was then added and stirred for 45 minutes. The mixture was then cooled to 50°C in a water bath, and 3.0 g of ethanol, a reaction terminator, was added. The reaction was terminated at 50°C for 30 minutes. After cooling the reaction solution, excess BDI and butyl acetate were removed by thin-film distillation (conditions: 110°C, 0.04 kPa), yielding 62 g of polyisocyanate composition P-2. P-2 contained 4.2% by mass of the compound (Cy-3) represented by formula (4) and 57.2% by mass of mononuclear isocyanurate.
[0115] Example 3: 500 g of BDI was charged into a 1 L four-neck flask equipped with a stirrer, thermometer, condenser, and nitrogen gas inlet tube. The mixture was heated to 100°C, and 5.0 g of hexamethyldisilazane, an isocyanurate catalyst, was added. The mixture was then heated to 120°C and stirred for 1.7 hours. 500 g of butyl acetate was then added and stirred for 80 minutes. The mixture was then cooled to 50°C in a water bath, and 3.0 g of ethanol, a reaction terminator, was added. The reaction was terminated at 50°C for 30 minutes. After cooling the reaction solution, excess BDI and butyl acetate were removed by thin-film distillation (conditions: 110°C, 0.04 kPa), yielding 62 g of polyisocyanate composition P-3. P-3 contained 8.3% by mass of the compound (Cy-3) represented by formula (4) and 54.5% by mass of mononuclear isocyanurate.
[0116] Example 4 A 300 mL three-neck flask equipped with a stirrer and a nitrogen gas inlet tube was charged with 150 g of C-HXLV (HDI-based isocyanurate composition, manufactured by Tosoh Corporation) and 0.75 g of Cy-1, and the mixture was stirred for 0.5 hours to obtain polyisocyanate composition P-4. P-4 contained 4.5 mass % of compound (Cy-1) represented by formula (2) and 63.9 mass % of isocyanurate mononuclear compounds.
[0117] Example 5 500 g of BDI was charged into a 1 L four-neck flask equipped with a stirrer, thermometer, condenser, and nitrogen gas inlet tube, and the mixture was heated to 100°C. 5.0 g of hexamethyldisilazane, an isocyanurate catalyst, was added, and the mixture was heated to 120°C and stirred for 1.7 hours. The mixture was then cooled to 50°C in a water bath, and 3.0 g of ethanol, a reaction terminator, was added, and the reaction was stopped at 50°C for 30 minutes. After cooling the reaction solution, excess BDI was removed by thin-film distillation (conditions: 110°C, 0.04 kPa), yielding 62 g of a polyisocyanate composition. 150 g of the resulting polyisocyanate composition and 1.5 g of Cy-2 were charged into a 300 mL three-neck flask equipped with a stirrer and nitrogen gas inlet tube, and the mixture was stirred for 0.5 hours to yield P-5. P-5 contained 8.9% by mass of the compound (Cy-2) represented by formula (3) and 54.6% by mass of an isocyanurate mononuclear compound.
[0118] Comparative Example 1: 500 g of BDI was charged into a 1 L four-neck flask equipped with a stirrer, thermometer, condenser, and nitrogen gas inlet tube. The mixture was heated to 100°C, and 5.0 g of hexamethyldisilazane, an isocyanurate catalyst, was added. The mixture was then heated to 150°C and stirred for 1.0 hour. The mixture was then cooled to 50°C in a water bath, and 3.0 g of ethanol, a reaction terminator, was added. The reaction was terminated at 50°C for 30 minutes. After cooling the reaction solution, excess BDI was removed by thin-film distillation (conditions: 110°C, 0.04 kPa), yielding 65 g of polyisocyanate composition P-6. P-6 contained 0.08% by mass of the compound (Cy-3) represented by formula (4) and 61.1% by mass of mononuclear isocyanurate.
[0119] Comparative Example 2 A 300 mL three-neck flask equipped with a stirrer and a nitrogen gas inlet tube was charged with 150 g of C-HXLV and 3.0 g of Cy-1, and the mixture was stirred for 0.5 hours to obtain polyisocyanate composition P-7. P-7 contained 16.5 mass% of compound (Cy-1) represented by formula (2) and 55.9 mass% of a mononuclear isocyanurate.
[0120] <Comparative Example 3> A 1 L four-neck flask equipped with a stirrer, thermometer, condenser, and nitrogen gas inlet tube was charged with 500 g of BDI and 500 g of butyl acetate, heated to 100 ° C, and 7.5 g of hexamethyldisilazane, an isocyanurate catalyst, was added. The mixture was then heated to 120 ° C and stirred for 2.0 hours. The mixture was then cooled to 50 ° C in a water bath, and 4.5 g of ethanol, a reaction terminator, was added, and the reaction was stopped at 50 ° C for 30 minutes. After cooling the reaction solution, excess BDI and butyl acetate were removed by thin-film distillation (conditions: 110 ° C, 0.04 kPa), yielding 60 g of polyisocyanate composition P-8. P-8 contained 21.0 mass% of the compound (Cy-3) represented by formula (4) and 41.2 mass% of mononuclear isocyanurate.
[0121] Comparative Example 4: A 1 L four-neck flask equipped with a stirrer, thermometer, condenser, and nitrogen gas inlet tube was charged with 500 g of 1,6-hexane diisocyanate (HDI) and 500 g of butyl acetate. The mixture was heated to 100 ° C., and 7.5 g of hexamethyldisilazane, an isocyanurate catalyst, was added. The mixture was then heated to 120 ° C. and stirred for 2.0 hours. The mixture was then cooled to 50 ° C. in a water bath, and 4.5 g of ethanol, a reaction terminator, was added. The reaction was terminated at 50 ° C. for 30 minutes. After cooling the reaction solution, excess HDI and butyl acetate were removed by thin-film distillation (conditions: 130 ° C., 0.04 kPa), yielding 61 g of polyisocyanate composition P-9. P-9 contained 65.4 mass% isocyanurate mononuclear compounds, but did not contain cyclic compounds.
[0122] <Preparation of Two-Component Coating Composition and Evaluation of Surface Smoothness> A coating composition comprising the obtained polyisocyanate composition and acrylic polyol was prepared, and then a coating film was formed using the coating composition. The surface smoothness of the formed coating film was evaluated. Specifically, an acrylic polyol (trade name: Acrydic A-801, hydroxyl value: 50 mg KOH / g resin, solids content: 50 mass%, manufactured by DIC Corporation) and a polyisocyanate composition were blended so that the equivalent ratio of hydroxyl groups to isocyanate groups was 1:1, and then butyl acetate was added to prepare a coating composition with a coating solids content of 40 mass%. The resulting coating composition was then applied to a steel plate (JIS G3141, trade name: SPCC-SB, treatment method: PF-1077, manufactured by Paltec Co., Ltd.) to a resin film thickness of 20 μm. The coating was then dried for 1 hour in an environment of 23°C and 50% relative humidity, and then heat-treated in a dryer at 150°C for 30 minutes. Subsequently, the coating was cured for at least 3 days in an environment of 23°C and 50% relative humidity to obtain a coating film. The arithmetic mean roughness of the coating film was then measured in accordance with JIS B0601 using a scanning white light interference microscope VS1530 (trade name, manufactured by Hitachi High-Technologies Corporation). The surface smoothness of the coating film was evaluated based on the arithmetic mean roughness of Comparative Example 4. The results are shown in Table 1.
[0123]
[0124] As shown in Table 1, the coating films prepared from the polyisocyanate compositions P-1 to P-5 had good surface smoothness. From these results, the polyisocyanate compositions of Examples 1 to 5 were polyisocyanate compositions that contributed to the preparation of coating films with excellent surface smoothness.
Claims
1. A composition comprising a polyisocyanate, wherein the polyisocyanate comprises a derivative derived from an aliphatic diisocyanate, and the content of a cyclic compound represented by the following formula (1) is 0.1 to 15 mass % relative to the total amount of the composition. [In formula (1), n is an integer from 1 to 6, and R 1 and R 2 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.
2. The composition of claim 1, wherein said derivative comprises an isocyanurate derived from an aliphatic diisocyanate.
3. The composition of claim 1 or 2, wherein the aliphatic diisocyanate comprises butane diisocyanate.
4. The above R 1 and the R 2 are each independently a hydrogen atom, an aliphatic group having 1 to 20 carbon atoms, an alicyclic group having 3 to 20 carbon atoms, or an aromatic group having 6 to 20 carbon atoms, and the aliphatic group, the alicyclic group, and the aromatic group may be substituted with a substituent and may contain one or more atoms selected from the group consisting of an oxygen atom, a nitrogen atom, and a sulfur atom.
5. The above R 1 and the R 2 The composition according to claim 1 or 2, wherein one of the groups is a hydrogen atom and the other is a monovalent organic group having 1 to 20 carbon atoms.
6. A curing agent for forming a polyurethane resin comprising the composition of claim 1.
7. A polyurethane resin-forming composition comprising the composition according to claim 1 and a polyol.
8. A coating composition comprising the polyurethane resin-forming composition according to claim 7.
9. A coating film comprising a cured product of the coating composition according to claim 8.
10. A surface smoothing agent for polyurethane coatings, comprising a cyclic compound represented by the following formula (1): [In formula (1), n is an integer from 1 to 6, and R 1 and R 2are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.
Citation Information
Patent Citations
Polyisocyanate composition, polyurethane resin and paint
JP6482657B2
Thermosetting resin composition
JP1981151720A
Aqueous coating composition
JP1990276877A
Preparation of polyisocyanate highly including uretdione groups
JP1999228524A
Conductive hard coat composition
JP2005298624A