Method for producing medical instrument
The method of plasma treating a plastic cloth base material and reacting it with a specific copolymer creates a durable, flexible, and permeable biocompatible layer on medical devices, addressing the need for long-term antithrombotic properties and operability, especially in small diameter devices.
Patent Information
- Application Number
- PCT/JP2024/008190
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-03
AI Technical Summary
Medical devices, particularly those in contact with blood, face challenges in maintaining antithrombotic properties over time and ensuring operability, especially in small diameters where stenosis or occlusion can occur, requiring a technique that balances biocompatibility and durability.
A method involving plasma treatment of a plastic cloth base material to generate hydroxyl groups, followed by reaction with a copolymer containing structural units derived from reactive monomers and (meth)acrylic acid esters, forming a biocompatible layer that inhibits blood clot formation and platelet adhesion, while allowing flexibility and permeability.
The method achieves durable antithrombotic properties and improved operability, maintaining patency even in smaller diameter medical devices by forming a strong, flexible, and permeable biocompatible layer that reduces the risk of stenosis and occlusion.
Smart Images

Figure JP2024008190_03102024_PF_FP_ABST
Abstract
Description
Manufacturing method of medical devices
[0001] The present invention relates to a method for manufacturing a medical device.
[0002] In recent years, medical materials using various polymeric materials have been investigated, and their use in artificial kidney membranes, plasma separation membranes, catheters, stents, artificial lung membranes, artificial blood vessels, adhesion prevention membranes, artificial skin, and other applications is anticipated. In these applications, synthetic polymeric materials, which are foreign to the living body, are used in contact with biological tissues and body fluids such as blood. Therefore, medical materials must be biocompatible. The biocompatibility required of medical materials varies depending on their purpose and method of use, but medical materials that come into contact with blood are required to have properties such as inhibition of the blood coagulation system, inhibition of platelet adhesion and activation, and inhibition of complement system activation (antithrombotic properties).
[0003] Typically, antithrombogenicity is imparted to a medical device by coating the substrate constituting the medical device with an antithrombogenic material, or by fixing an antithrombogenic material to the surface of the substrate. For example, Japanese Patent Laid-Open Publication No. 4-152952 discloses a medical device having, on the surface of its substrate, a synthetic polymer (antithrombogenic material) that simultaneously satisfies biocompatibility, such as inhibiting platelet adhesion and activation and inhibiting activation of the complement system, and having affinity for in vivo tissues.
[0004] The invention disclosed in Japanese Patent Laid-Open No. 4-152952 shows good results in terms of inhibiting platelet adhesion and activation.
[0005] In some of these medical devices, in order to maintain excellent antithrombotic properties for a long period of time, it is required that the antithrombotic material be able to be maintained on the substrate for a long period of time (i.e., that an antithrombotic coating with excellent durability be able to be formed).
[0006] For example, implantable medical devices (especially those with small diameters) such as artificial blood vessels, stent grafts, and covered stents are prone to a decline in patency due to stenosis or occlusion, and are therefore particularly required to maintain antithrombogenicity over a long period of time. Furthermore, as medical devices have become smaller and thinner in recent years, there is a demand for technology that enables smooth insertion and placement of medical devices (with less load) in areas of narrow inner diameters or bent portions of biological lumens.
[0007] Therefore, the present invention has been made in view of the above circumstances, and an object of the present invention is to provide a technology that achieves both antithrombotic properties and operability of a medical device.
[0008] The present inventors have conducted extensive research to solve the above problems, and as a result have found that the above problems can be solved by subjecting a plastic fabric substrate to plasma treatment to generate hydroxyl groups on the surface, and then reacting these hydroxyl groups with a copolymer reactive with hydroxyl groups, thereby completing the present invention.
[0009] That is, the above objects can be achieved by the present invention having the following configuration, and the present invention includes the following aspects and configurations.
[0010] One aspect of the present invention is a method for producing a medical device comprising: 1. a plastic fabric substrate; and a biocompatible layer carried on at least a portion of the plastic fabric substrate, wherein the biocompatible layer comprises a structural unit A derived from a monomer having a reactive group that reacts with a hydroxyl group in the molecule, and a polymerizable compound represented by the following formula (I):
[0011]
[0012] In the above formula (I), R 1 represents a hydrogen atom or a methyl group; X represents a group of the formula: —O—(R 2 O) m -R 3 or a tetrahydrofurfuryloxy group, in which R 2 each independently represents a linear or branched alkylene group having 1 to 4 carbon atoms; R 3represents a linear or branched alkyl group having 1 to 4 carbon atoms, and m represents an integer of 1 to 5; and the plastic fabric substrate is subjected to a plasma treatment to generate hydroxyl groups on the surface of the plastic fabric substrate, and the hydroxyl groups are reacted with the reactive groups.
[0013] 2. In the production method described in 1 above, it is preferable that the copolymer is a random copolymer and has a carboxyl group at at least one end.
[0014] 3. In the production method described in 2 above, the carboxyl group is preferably derived from at least one compound selected from the group consisting of 4,4'-azobis(4-cyanovaleric acid) and 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]tetrahydrate.
[0015] 4. In the production method described in 1 above, the copolymer is preferably a block copolymer composed of structural units A and B.
[0016] 5. In the manufacturing method according to any one of the above 1. to 4., the reactive functional group is a primary amino group (—NH 2 ) or an epoxy group.
[0017] 6. In the production method described in any one of 1. to 5. above, the structural unit A is preferably derived from at least one monomer selected from the group consisting of aminomethyl acrylamide, aminomethyl methacrylamide, aminoethyl acrylamide, aminoethyl methacrylamide, aminopropyl acrylamide, aminopropyl methacrylamide (APMA), aminobutyl acrylamide, aminobutyl methacrylamide, and salts thereof, as well as glycidyl acrylate, glycidyl methacrylate (GMA), 3,4-epoxycyclohexylmethyl acrylate, 3,4-epoxycyclohexylmethyl methacrylate, β-methylglycidyl acrylate, and β-methylglycidyl methacrylate.
[0018] 7. In the manufacturing method described in any one of 1. to 6. above, the structural unit B is preferably derived from at least one monomer selected from the group consisting of methoxymethyl acrylate, methoxyethyl acrylate (MEA), methoxypropyl acrylate, ethoxymethyl acrylate, ethoxyethyl acrylate, ethoxypropyl acrylate, ethoxybutyl acrylate, propoxymethyl acrylate, butoxyethyl acrylate, methoxybutyl acrylate, methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, propoxymethyl methacrylate, and butoxyethyl methacrylate.
[0019] 8. In the manufacturing method described in any one of 1. to 7. above, the plastic is preferably at least one selected from the group consisting of polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), and polybutylene terephthalate (PBT).
[0020] 9. In the manufacturing method according to any one of the above items 1 to 8, the medical device is preferably an artificial blood vessel, a stent graft, a covered stent, or a catheter.
[0021] FIG. 1 is a partial cross-sectional view schematically illustrating the structure of a representative embodiment of a medical device according to the present invention. FIG. 2 is a partial cross-sectional view schematically illustrating an example of a different structure as an application example of the embodiment of FIG. 1. FIGS. 3A to 3D show SEM images of the surfaces of samples (1) to (2). FIGS. 3E to 3H show SEM images of the surfaces of samples (3) to (4). FIGS. 4A to 4D show SEM images of the surfaces of samples (1) to (4) after antithrombogenicity evaluation. FIGS. 5A and 5B show SEM images of the surface of sample (5). FIG. 6 shows an SEM image of the surface of sample (6) after antithrombogenicity evaluation.
[0022] The present invention provides a method for producing a medical device comprising a plastic fabric substrate and a biocompatible layer (antithrombogenic layer) supported on at least a portion of the plastic fabric substrate, the biocompatible layer comprising a copolymer having a structural unit A derived from a monomer having a reactive group reactive with a hydroxyl group in its molecule and a structural unit B derived from a (meth)acrylic acid ester represented by the following formula (I), the method comprising treating the plastic fabric substrate with plasma to generate hydroxyl groups on the surface of the plastic fabric substrate and reacting the hydroxyl groups with the reactive groups. This invention provides a technology for achieving both antithrombogenicity and ease of use in medical devices.
[0023]
[0024] In the above formula (I), R 1 represents a hydrogen atom or a methyl group; X represents a group of the formula: —O—(R 2 O) m -R 3 or a tetrahydrofurfuryloxy group, in which R 2 each independently represents a linear or branched alkylene group having 1 to 4 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 4 carbon atoms; and m represents an integer of 1 to 5.
[0025] Herein, a medical device having the above configuration is also referred to simply as the "medical device according to the present invention" or "medical device." Furthermore, herein, the structural unit A derived from a monomer having in its molecule a reactive group that reacts with a hydroxyl group is also referred to simply as the "structural unit A according to the present invention" or "structural unit A." Herein, the structural unit B derived from the (meth)acrylic acid ester represented by formula (I) above is also referred to simply as the "structural unit B according to the present invention" or "structural unit B." Herein, a copolymer having structural units A and B is also referred to simply as the "copolymer according to the present invention" or "copolymer."
[0026] In this specification, the term "hydroxyl group" refers to a group having an -OH group. Therefore, the hydroxyl group includes a carboxyl group (-COOH) in addition to a hydroxyl group (-OH). That is, the hydroxyl group may be contained in the form of a carboxyl group (-COOH).
[0027] In this specification, when a certain structural unit is defined as being "derived from" a certain monomer, it means that the structural unit is a structural unit that is generated by cleavage of one of the polymerizable unsaturated double bonds of the corresponding monomer.
[0028] As used herein, the term "(meth)acrylic" encompasses both acrylic and methacrylic. Thus, for example, the term "(meth)acrylic acid" encompasses both acrylic acid and methacrylic acid. Similarly, the term "(meth)acryloyl" encompasses both acryloyl and methacryloyl. Thus, for example, the term "(meth)acryloyl group" encompasses both acryloyl and methacryloyl groups. Similarly, the term "(meth)acrylate" encompasses both acrylate and methacrylate. Thus, for example, the term "alkoxyalkyl(meth)acrylate" encompasses both alkoxyalkylacrylate and alkoxyalkylmethacrylate.
[0029] In this specification, the term "X to Y" indicating a range includes X and Y and means "X or more and Y or less." Furthermore, "A and / or B" includes each of A and B and all combinations of one or more thereof, and specifically means at least one of A and B, and also means A, B, and a combination of A and B. Furthermore, unless otherwise specified, measurements of operations and physical properties are performed under conditions of room temperature (20 to 25°C) and a relative humidity of 40 to 50% RH.
[0030] Hereinafter, embodiments of the present invention will be described. Note that the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the claims. Furthermore, the embodiments described in this specification can be arbitrarily combined to form other embodiments. The dimensional proportions in the drawings are exaggerated for the convenience of explanation and may differ from the actual proportions. Furthermore, when embodiments of the present invention are described with reference to the drawings, the same elements are given the same reference numerals in the description of the drawings, and duplicate explanations will be omitted.
[0031] Throughout this specification, singular expressions should be understood to include the plural concept unless otherwise specified. Therefore, singular articles (e.g., "a," "an," "the," etc. in English) should be understood to include the plural concept unless otherwise specified. Furthermore, terms used in this specification should be understood to be used in the sense commonly used in the art unless otherwise specified. Therefore, unless otherwise defined, all technical and scientific terms used in this specification have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. In case of conflict, the present specification (including definitions) will prevail.
[0032] [Medical Device] Hereinafter, the configuration of a medical device according to one embodiment of the present invention will be described with reference to the accompanying drawings.
[0033] Fig. 1 is a partial cross-sectional view schematically illustrating the structure of a representative embodiment of a medical device according to the present invention, and Fig. 2 is a partial cross-sectional view schematically illustrating an example of a different structure as an application example of this embodiment.
[0034] As shown in Figures 1 and 2, a medical device 100 according to one embodiment of the present invention comprises a plastic fabric substrate 10 and a biocompatible layer (antithrombogenic layer) 11 supported on at least a portion of the plastic fabric substrate. The medical device 100 of this embodiment comprises the plastic fabric substrate (also simply referred to as "substrate") 10 and the biocompatible layer (antithrombogenic layer) 11 directly laminated in this order. That is, the substrate 10 and the biocompatible layer (antithrombogenic layer) 11 are laminated adjacently in this order. The biocompatible layer (antithrombogenic layer) 11 is supported on at least a portion of the substrate 10. In this specification, "supported" refers to a layer (upper layer) being immobilized in a manner that prevents it from easily separating (peeling off) from the surface of the underlying layer. Specifically, the state in which the biocompatible layer (antithrombogenic layer) is "supported" on the substrate may mean a state in which the copolymer is bonded (immobilized) to the surface of the substrate to form a biocompatible layer, a state in which the copolymer (biocompatible layer) is deposited on the surface of the substrate, or a state in which the copolymer (biocompatible layer) is impregnated into the surface of the substrate.
[0035] From the viewpoint of maintaining antithrombotic properties for a long period of time, the preferred form of "support" is a state in which the surface of the biocompatible layer (particularly the reactive groups of the copolymer constituting the biocompatible layer) and the surface of the plastic fabric substrate (particularly the hydroxyl groups generated by plasma treatment) are physically and / or chemically bonded, and a more preferred form is a state in which they are chemically bonded. Note that "chemically bonded" here refers to a state in which at least a portion of the surface of the biocompatible layer and at least a portion of the surface of the plastic fabric substrate are bonded by covalent bonds, ionic bonds, hydrogen bonds, intermolecular forces, etc.
[0036] Furthermore, in this specification, the phrase "a biocompatible layer (antithrombogenic layer) is supported on at least a portion of the plastic fabric substrate" is used because, in artificial blood vessels, stent grafts, covered stents, catheters, and the like, which are examples of uses of medical devices, it is not necessary to impart antithrombogenicity to the entire surface (entire surface) of these medical devices; rather, it is sufficient that the biocompatible layer (antithrombogenic layer) is supported only on the surface portion (which may be a portion or the entire surface) that is required to have antithrombogenicity. For this reason, it is preferable that the biocompatible layer (antithrombogenic layer) is supported on at least the portion of the substrate 10 that comes into contact with blood (e.g., the inner wall of an artificial blood vessel). For example, when the medical device is an artificial blood vessel, stent graft, covered stent, or catheter, it is preferable that the biocompatible layer (antithrombogenic layer) is supported (formed) on the entire surface of the substrate.
[0037] <<Plastic Fabric Substrate (Plastic Fabric Substrate Layer)>> A medical device according to one embodiment of the present invention has a plastic fabric substrate (plastic fabric substrate layer, polymer substrate). As the plastic fabric substrate, an optimal substrate can be appropriately selected depending on the properties (e.g., mechanical strength) required for medical devices such as artificial blood vessels, stent grafts, covered stents, and catheters. For example, a plastic fabric substrate having properties required for a substrate, such as mechanical strength, flexibility, and smoothness, is preferred.
[0038] The substrate 10 may have at least its surface made of plastic (polymer material). For example, as shown in FIG. 1, the entire substrate may be made of plastic (polymer material). Alternatively, as shown in FIG. 2, the substrate may have a structure in which the surface of a substrate core portion 10a formed of a hard reinforcing material such as a metal or ceramic material is coated with a plastic (polymer material) that is more flexible than the reinforcing material, such as a metal material, by an appropriate method (a conventionally known method such as dipping, spraying, coating, or printing), thereby forming a substrate surface layer 10b. Alternatively, the substrate 10 may be formed by combining (by an appropriate reaction process) the reinforcing material of the substrate core portion 10a and the plastic (polymer material) of the substrate surface layer 10b. Therefore, the substrate core portion 10a may be a multilayer structure formed by laminating different materials in multiple layers, or a structure (composite) in which components formed of different materials are joined together for each portion of the medical device. Furthermore, a separate middle layer (not shown) may be formed between the substrate core portion 10a and the substrate surface layer 10b. Furthermore, as for the substrate surface layer 10b, as long as its surface is made of plastic (polymer material), it may be a multilayer structure formed by laminating multiple layers of different materials, or a structure (composite) in which components formed of different materials for each part of the medical device are joined together.
[0039] The material (polymer material) constituting (forming) the substrate 10 and the substrate surface layer 10b is not particularly limited, and polymer materials commonly used in medical devices such as artificial blood vessels, stent grafts, covered stents, and catheters can be used. Specific examples include polyamide resins such as nylon 6, nylon 11, nylon 12, and nylon 66 (all registered trademarks); polyethylenes such as linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), high-density polyethylene (HDPE), and modified polyethylene; polyolefin resins such as polypropylene; polyester resins such as polyethylene terephthalate (PET); styrene resins such as polystyrene; cyclic polyolefin resins, modified polyolefin resins, epoxy resins, urethane resins, diallyl phthalate resins (allyl resins), polycarbonate resins, and fluororesins such as ePTFE (expanded polyethylene tetrafluoroethylene); amino resins (urea resins, melamine resins, benzoguanamine resins), acrylic resins, polyacetal resins, vinyl acetate resins, phenolic resins, vinyl chloride resins, silicone resins, polyether resins such as polyether ether ketone (PEEK), and polyimide resins. These may be used alone or in combination. The polymer material can be selected appropriately depending on the intended use of the medical device. Polymeric materials (plastics) constituting (forming) the substrates of artificial blood vessels, stent grafts, covered stents, catheters, and other applications preferably contain polyester resins and / or fluororesins. Furthermore, from the viewpoint of mechanical strength, the polymeric materials (plastics) more preferably contain polyester resins. Examples of such polyester resins include polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), and polybutylene terephthalate (PBT).Therefore, the polymeric material (plastic) constituting (forming) the substrate 10 or the substrate surface layer 10b is preferably at least one selected from the group consisting of polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), and polybutylene terephthalate (PBT), and is more preferably polyethylene terephthalate (PET).
[0040] The material that can be used for the substrate core portion 10a is not particularly limited, and a reinforcing material that can fully exhibit the optimal function of the substrate core portion 10a may be appropriately selected depending on the intended use of the medical device (e.g., artificial blood vessel). Examples of the material include, but are not limited to, various stainless steels (SUS) such as SUS304, SUS316L, SUS420J2, and SUS630; various metal materials such as gold, platinum, silver, copper, nickel, cobalt, titanium, iron, aluminum, tin, and alloys thereof (e.g., nickel-titanium alloy, cobalt-chromium alloy, zinc-tungsten alloy, etc.); inorganic materials such as various ceramic materials; and metal-ceramic composites.
[0041] Alternatively, the substrate core portion 10a may be made of a polymeric material other than the plastic (polymeric material) that forms (constitutes) the substrate surface layer 10b. Examples of such polymeric materials are not particularly limited, and include the same materials as those described above. These may be used alone or in combination of two or more.
[0042] Preferably, the substrate 10 contains or is made of a plastic (polymer material), or the substrate surface layer 10b contains or is made of a plastic (polymer material). More preferably, the substrate 10 is made of a plastic (polymer material), or the substrate surface layer 10b is made of a plastic (polymer material).
[0043] The shape of the substrate 10 is not particularly limited, and may be appropriately selected depending on the mode of use, such as a sheet, a film, a tube, a shape having multiple branched tubes such as a bifurcated shape (for example, a Y-shape), etc. The substrate 10 is a fabric made of fibers (yarns), and examples of fabrics include woven fabrics, knitted fabrics, nonwoven fabrics, etc., and may be in any form.
[0044] <Biocompatible Layer (Antithrombogenic Layer)> The biocompatible layer (antithrombogenic layer) according to the present invention comprises a copolymer having a structural unit A derived from a monomer having in its molecule a reactive group that reacts with a hydroxyl group, and a structural unit B derived from a (meth)acrylic acid ester represented by the above formula (I). The biocompatible layer (antithrombogenic layer) may be in the form of a single layer or a laminate of two or more layers. Preferably, the biocompatible layer (antithrombogenic layer) is in the form of a single layer.
[0045] In this specification, "biocompatibility" varies depending on the purpose and method of use, but medical materials used as materials that come into contact with blood are required to have the following properties: inhibition of the blood coagulation system, inhibition of platelet adhesion and activation, inhibition of activation of the complement system, and affinity with in vivo tissues (antithrombogenicity). Therefore, in this specification, the term "biocompatible layer" encompasses an antithrombogenic layer.
[0046] The structural unit A is derived from a monomer (hereinafter simply referred to as "monomer A") having a reactive group in the molecule that reacts with a hydroxyl group. The reactive group in the structural unit A reacts with the hydroxyl group (hydroxyl group (-OH) and / or carboxyl group (-COOH)) generated on the surface of the plastic fabric substrate by plasma treatment. This allows the biocompatible layer (antithrombogenic layer) to be firmly immobilized (bonded, supported) on the plastic fabric substrate.
[0047] The reactive group present in the structural unit A may have any structure as long as it is a group that can react with a hydroxyl group (hydroxyl group (-OH) and / or carboxyl group (-COOH)). Specifically, a primary amino group (-NH 2 ), secondary amino groups (-NHZ (wherein Z is a linear or branched alkyl group having 1 to 8 carbon atoms)), tertiary amino groups (-NZ 2(each Z is independently a linear or branched alkyl group having 1 to 8 carbon atoms) and an epoxy group. When the reactive group is a secondary or tertiary amino group, examples of Z include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a sec-butyl group, a tert-butyl group, an isobutyl group, an n-pentyl group, an isopentyl group, a neopentyl group, a 1,2-dimethylpropyl group, an n-hexyl group, a 1,3-dimethylbutyl group, a 1-iso-propylpropyl group, a 1,2-dimethylbutyl group, an n-heptyl group, an n-octyl group, and a 2-ethylhexyl group. Of these, from the viewpoint of reactivity with hydroxyl groups (hydroxyl groups (-OH) and / or carboxyl groups (-COOH)), a primary amino group (-NH 2 ), epoxy group (-C 2 H 3 O) is preferred, and primary amino groups (—NH 2 ), a glycidyl group (—CH 2 -C 2 H 3 That is, in a preferred embodiment of the present invention, the reactive groups are a primary to tertiary amino group and an epoxy group (—C 2 H 3 In a more preferred embodiment of the present invention, the reactive group comprises at least one selected from the group consisting of a primary amino group (—NH 2 ) and epoxy groups (-C 2 H 3 In a further preferred embodiment of the present invention, the reactive group comprises at least one of a primary amino group (-NH 2 ) or an epoxy group (-C 2 H 3 In a particularly preferred embodiment of the invention, the reactive group is a primary amino group (-NH 2 ) or a glycidyl group (—CH 2 -C 2 H 3 O).
[0048] Monomer A has an acryloyl group (CH 2 ═CH—C(═O)—), methacryloyl group (CH 2 =C(CH 3)-C(=O)-), vinyl group (CH 2 It is preferable that the alkyl group further contains an ethylenically unsaturated group such as ═CH—, and it is more preferable that the alkyl group further contains an acryloyl group or a methacryloyl group.
[0049] For example, when the monomer A has a primary amino group and an ethylenically unsaturated group, specific examples of the monomer A include monomers represented by the following formula (II) and formula (III) and salts thereof.
[0050]
[0051] In the above formula (II), R 4 represents a hydrogen atom or a methyl group, and p represents an integer of 0 to 4;
[0052]
[0053] In the above formula (III), R 5 represents a hydrogen atom or a methyl group; and q represents an integer of 0 to 4.
[0054] In the above, the term "salts thereof" refers to compounds formed by neutralizing the charge of a cation and an anion, and preferably refers to compounds formed by neutralizing the charge of a primary amino group (-NH 2 ) is an acid (H + X - ) refers to a compound that has been salified (neutralized) by . Specific examples include hydrochlorides, phosphates, ribonucleic acid salts, tartrates, lactates, etc. Among these, hydrochlorides are preferred.
[0055] In the above formula (II), R 4 is a hydrogen atom or a methyl group, and preferably, R 4 is a methyl group.
[0056] In the above formula (II), p is an integer of 0 to 4. From the viewpoint of further imparting antithrombotic properties, p is preferably an integer of 1 to 4, more preferably an integer of 2 to 4, even more preferably 2 or 3, and particularly preferably 3.
[0057] In the above formula (III), R 5is a hydrogen atom or a methyl group, and preferably, R 5 is a methyl group.
[0058] In the above formula (III), q is an integer of 0 to 4. From the viewpoint of further imparting antithrombotic properties, q is preferably an integer of 1 to 4, more preferably an integer of 2 to 4, even more preferably 2 or 3, and particularly preferably 3.
[0059] From the viewpoint of further imparting antithrombotic properties, the monomer A is preferably one or more selected from the monomers represented by the above formula (II) and salts thereof.
[0060] Specific examples of the monomer represented by formula (II) include, but are not limited to, aminomethylacrylamide, aminomethylmethacrylamide, aminoethylacrylamide, aminoethylmethacrylamide, aminopropylacrylamide, aminopropylmethacrylamide (APMA), aminobutylacrylamide, and aminobutylmethacrylamide. Among these, from the viewpoints of further improving adhesion to plastic fabric substrates (immobilization to plastic fabric substrates) (reactivity with hydroxyl groups) and further imparting antithrombogenicity, it is preferred that monomer A comprise at least one selected from the group consisting of aminomethylacrylamide, aminomethylmethacrylamide, aminoethylacrylamide, aminoethylmethacrylamide, aminopropylacrylamide, aminopropylmethacrylamide (APMA), aminobutylacrylamide, aminobutylmethacrylamide, and salts thereof. Furthermore, it is even more preferred that monomer A comprise at least one selected from the group consisting of aminoethylacrylamide, aminoethylmethacrylamide, aminopropylacrylamide, aminopropylmethacrylamide (APMA), and salts thereof. Furthermore, it is particularly preferable that the monomer A contains at least one selected from the group consisting of aminopropyl acrylamide, aminopropyl methacrylamide (APMA), and salts thereof.Moreover, it is most preferable that the monomer A is selected from aminopropyl methacrylamide (APMA) and salts thereof.
[0061] For example, when the monomer A has an epoxy group and an ethylenically unsaturated group, specific examples of the monomer A include (meth)acrylic acid esters having a glycidyl group (epoxy group), such as glycidyl acrylate, glycidyl methacrylate (GMA), 3,4-epoxycyclohexylmethyl acrylate, 3,4-epoxycyclohexylmethyl methacrylate, β-methylglycidyl acrylate, and β-methylglycidyl methacrylate; and vinyl ethers having a glycidyl group (epoxy group), such as allyl glycidyl ether, but are not limited to these. Among these, from the viewpoints of further improving adhesion to plastic fabric substrates (immobilization to plastic fabric substrates) (reactivity with hydroxyl groups) and ease of control of polymerization during copolymer preparation, it is preferable that monomer A contains at least one selected from the group consisting of glycidyl acrylate, glycidyl methacrylate (GMA), 3,4-epoxycyclohexylmethyl acrylate, 3,4-epoxycyclohexylmethyl methacrylate, β-methylglycidyl acrylate, and β-methylglycidyl methacrylate. Furthermore, it is more preferable that monomer A contains at least one selected from the group consisting of glycidyl acrylate and glycidyl methacrylate. Furthermore, it is even more preferable that monomer A contains glycidyl acrylate or glycidyl methacrylate, particularly preferably glycidyl methacrylate, and most preferably glycidyl methacrylate.
[0062] That is, in a preferred embodiment of the present invention, the structural unit A is derived from at least one monomer selected from the group consisting of aminomethyl acrylamide, aminomethyl methacrylamide, aminoethyl acrylamide, aminoethyl methacrylamide, aminopropyl acrylamide, aminopropyl methacrylamide (APMA), aminobutyl acrylamide, aminobutyl methacrylamide, and salts thereof, as well as glycidyl acrylate, glycidyl methacrylate (GMA), 3,4-epoxycyclohexylmethyl acrylate, 3,4-epoxycyclohexylmethyl methacrylate, β-methylglycidyl acrylate, and β-methylglycidyl methacrylate. In a more preferred embodiment of the present invention, the structural unit A is derived from at least one monomer selected from the group consisting of aminoethyl acrylamide, aminoethyl methacrylamide, aminopropyl acrylamide, aminopropyl methacrylamide (APMA), and salts thereof, glycidyl acrylate, and glycidyl methacrylate. In a particularly preferred embodiment of the present invention, the structural unit A is derived from aminopropyl acrylamide or a salt thereof, aminopropyl methacrylamide (APMA) or a salt thereof, glycidyl acrylate, or glycidyl methacrylate (GMA). In a most preferred embodiment of the present invention, the structural unit A is derived from aminopropyl methacrylamide (APMA) or a salt thereof, or glycidyl methacrylate (GMA).
[0063] The structural unit A is preferably a structural unit derived from a monomer suitable for use as the monomer A. This configuration facilitates the formation of a stronger bond between the plastic fabric substrate and the biocompatible layer, and also has the advantage of being easy to manufacture.
[0064] The monomer A may be used alone or in combination of two or more. That is, the structural unit A may be a homopolymer type composed of a single structural unit, or a copolymer type composed of two or more structural units. When two or more types of the monomer A are used, the segment composed of the monomer A may be in the form of a block copolymer, a random copolymer, or an alternating copolymer.
[0065] The content of the structural unit A is preferably more than 5 mol% and less than 25 mol%, more preferably 9 mol% or more and 20 mol% or less, based on 100 mol% of all structural units constituting the copolymer. With such a composition, the copolymer sufficiently reacts with hydroxyl groups (-OH and / or -COOH) on the surface of the plastic fabric substrate via the reactive groups, allowing the biocompatible layer to bond more firmly to the plastic fabric substrate.
[0066] The copolymer according to the present invention has a structural unit B derived from an antithrombotic monomer B (a (meth)acrylic acid ester). Here, the term "antithrombotic monomer B" refers to a compound whose homopolymer exhibits antithrombotic properties, i.e., the property of reducing blood coagulation on a surface that comes into contact with blood.
[0067] Specifically, structural unit B is derived from a (meth)acrylic acid ester represented by the following formula (I) (hereinafter also referred to simply as "antithrombogenic monomer B" or "(meth)acrylic acid ester"). A copolymer containing structural unit B is excellent in biocompatibility (the effect of inhibiting and preventing platelet adhesion / adhesion and the effect of inhibiting and preventing platelet activation), particularly in the effect of inhibiting and preventing platelet adhesion / adhesion. Therefore, the presence of structural units A and B not only provides excellent antithrombogenicity, but also forms a strong bond between the plastic fabric substrate and the copolymer of the present invention, resulting in a medical device that can maintain its antithrombogenicity for a long period of time (excellent durability).
[0068]
[0069] The antithrombotic monomer B ((meth)acrylic acid ester) may be used alone or in combination of two or more types. That is, the structural unit B may be a homopolymer type constituted of a single structural unit, or a copolymer type constituted of two or more structural units. When two or more types of the antithrombotic monomer B ((meth)acrylic acid ester) are used, the segment constituted by the antithrombotic monomer B ((meth)acrylic acid ester) may be in the form of a block copolymer, a random copolymer, or an alternating copolymer.
[0070] In the above formula (I), R 1 represents a hydrogen atom or a methyl group. From the viewpoint of obtaining excellent biocompatibility (especially antithrombogenicity), R 1 is a hydrogen atom.
[0071] In the above formula (I), X is a group represented by the formula: —O—(R 2 O) m -R 3 or a tetrahydrofurfuryloxy group, wherein X is a tetrahydrofurfuryloxy group having the following structure:
[0072]
[0073] X is a group of the formula: -O-(R 2 O) m -R 3 When R is a group represented by 2 each independently represents a linear or branched alkylene group having 1 to 4 carbon atoms. 2 When there are a plurality of -O- (m is 2 or more), each -R 2 The O- may be the same or different. 2 Specific examples of the R include a methylene group, an ethylene group, a trimethylene group, a propylene group, and a tetramethylene group. 2are each independently more preferably a methylene group, an ethylene group, or a trimethylene group, particularly preferably an ethylene group or a trimethylene group, and most preferably an ethylene group. 2 O) m -R 3 In this case, R 3 represents a linear or branched alkyl group having 1 to 4 carbon atoms. Specific examples include linear or branched alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, and tert-butyl. Among these, from the viewpoint of obtaining superior antithrombotic properties, R 3 is preferably a linear or branched alkyl group having 1 to 3 carbon atoms, more preferably an alkyl group having 1 or 2 carbon atoms (methyl group, ethyl group), and particularly preferably a methyl group.
[0074] In the above formula (I), m is (-R 2 O—) groups and is an integer of 1 to 5. From the viewpoint of improving antithrombotic properties, m is preferably an integer of 1 to 3, more preferably 1 or 2, and particularly preferably 1.
[0075] In the above formula (I), X is —O—(R 2 O) m -R 3 or a tetrahydrofurfuryloxy group. Of these, from the viewpoint of obtaining superior antithrombotic properties, X is preferably —O—(R 2 O) m -R 3 From the same viewpoint, it is preferable that the antithrombotic monomer B ((meth)acrylic acid ester) is R 1 represents a hydrogen atom or a methyl group, and X is —O—(R 2 O) m -R 3 where R 2 represents a linear or branched alkylene group having 1 to 4 carbon atoms; R 3represents a linear or branched alkyl group having 1 to 3 carbon atoms, and m is 1 to 3. From the same viewpoint, the antithrombotic monomer B ((meth)acrylic acid ester) is preferably an alkoxyalkyl(meth)acrylate represented by the above formula (I), in which R 1 represents a hydrogen atom or a methyl group, and X is —O—(R 2 O) m -R 3 where R 2 represents a methylene group, an ethylene group, or a trimethylene group, and R 3 represents a methyl group or an ethyl group, and m is 1 or 2. From the same viewpoint, the antithrombotic monomer B ((meth)acrylic acid ester) is more preferably an alkoxyalkyl(meth)acrylate represented by the above formula (I) in which R 1 represents a hydrogen atom or a methyl group, and X is —O—(R 2 O) m -R 3 where R 2 represents an ethylene group or a trimethylene group, and R 3 represents a methyl group or an ethyl group, and m is 1. From the same viewpoint, the antithrombotic monomer B ((meth)acrylic acid ester) is particularly preferably an alkoxyalkyl(meth)acrylate represented by the above formula (I) in which R 1 represents a hydrogen atom or a methyl group, and X is —O—(R 2 O) m -R 3 where R 2 represents an ethylene group, and R 3 It is most preferable that the alkoxyalkyl(meth)acrylate is an alkoxyalkyl(meth)acrylate represented by the above formula (I) in which represents a methyl group and m is 1.
[0076] Specific examples of the antithrombotic monomer B represented by the above formula (I) include, but are not limited to, methoxymethyl acrylate, methoxyethyl acrylate (MEA), methoxypropyl acrylate, ethoxymethyl acrylate, ethoxyethyl acrylate (EEA), ethoxypropyl acrylate, ethoxybutyl acrylate, 2-(2-ethoxyethoxy)ethyl acrylate (EEEA), ethoxypropyl acrylate, ethoxybutyl acrylate, propoxymethyl acrylate, butoxyethyl acrylate, methoxybutyl acrylate, tetrahydrofurfuryl acrylate (THFA), methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, 2-(2-ethoxyethoxy)ethyl methacrylate, propoxymethyl methacrylate, butoxyethyl methacrylate, tetrahydrofurfuryl methacrylate, and the like. Of these, from the viewpoint of further improving the antithrombogenicity and further improving the durability (i.e., maintaining the antithrombogenicity for a longer period of time), it is preferable that the antithrombogenic monomer B contains at least one selected from the group consisting of methoxymethyl acrylate, methoxyethyl acrylate (MEA), ethoxymethyl acrylate, ethoxyethyl acrylate (EEA), 2-(2-ethoxyethoxy)ethyl acrylate (EEEA), tetrahydrofurfuryl acrylate (THFA), methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, 2-(2-ethoxyethoxy)ethyl methacrylate, and tetrahydrofurfuryl methacrylate.Furthermore, it is more preferable that the antithrombotic monomer B contains at least one selected from the group consisting of methoxymethyl acrylate, methoxyethyl acrylate (MEA), methoxypropyl acrylate, ethoxymethyl acrylate, ethoxyethyl acrylate, ethoxypropyl acrylate, ethoxybutyl acrylate, propoxymethyl acrylate, butoxyethyl acrylate, methoxybutyl acrylate, methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, propoxymethyl methacrylate, butoxyethyl methacrylate, and tetrahydrofurfuryl acrylate. Furthermore, it is particularly preferable that the antithrombotic monomer B is methoxyethyl acrylate and / or tetrahydrofurfuryl acrylate. Furthermore, it is most preferable that the antithrombotic monomer B is methoxyethyl acrylate. These monomers can be used alone or in combination of two or more.
[0077] That is, in one embodiment of the present invention, the structural unit B is derived from at least one monomer selected from the group consisting of methoxymethyl acrylate, methoxyethyl acrylate (MEA), methoxypropyl acrylate, ethoxymethyl acrylate, ethoxyethyl acrylate (EEA), ethoxypropyl acrylate, ethoxybutyl acrylate, 2-(2-ethoxyethoxy)ethyl acrylate (EEEA), ethoxypropyl acrylate, ethoxybutyl acrylate, propoxymethyl acrylate, butoxyethyl acrylate, methoxybutyl acrylate, tetrahydrofurfuryl acrylate (THFA), methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, 2-(2-ethoxyethoxy)ethyl methacrylate, propoxymethyl methacrylate, butoxyethyl methacrylate, and tetrahydrofurfuryl methacrylate. In a preferred embodiment of the present invention, the structural unit B is derived from at least one monomer selected from the group consisting of methoxymethyl acrylate, methoxyethyl acrylate (MEA), ethoxymethyl acrylate, ethoxyethyl acrylate (EEA), 2-(2-ethoxyethoxy)ethyl acrylate (EEEA), tetrahydrofurfuryl acrylate (THFA), methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, 2-(2-ethoxyethoxy)ethyl methacrylate, and tetrahydrofurfuryl methacrylate.In a preferred embodiment of the present invention, the structural unit B is derived from at least one monomer selected from the group consisting of methoxymethyl acrylate, methoxyethyl acrylate (MEA), methoxypropyl acrylate, ethoxymethyl acrylate, ethoxyethyl acrylate, ethoxypropyl acrylate, ethoxybutyl acrylate, propoxymethyl acrylate, butoxyethyl acrylate, methoxybutyl acrylate, methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, propoxymethyl methacrylate, butoxyethyl methacrylate, and tetrahydrofurfuryl acrylate. In a preferred embodiment of the present invention, the structural unit B is derived from methoxyethyl acrylate and / or tetrahydrofurfuryl acrylate. In a preferred embodiment of the present invention, the structural unit B is derived from methoxyethyl acrylate.
[0078] The content of the structural unit B is preferably more than 75 mol % and less than 95 mol %, and more preferably 80 mol % or more and 91 mol % or less, relative to 100 mol % of all structural units constituting the copolymer. With such a composition, the copolymer can exhibit sufficient antithrombotic properties.
[0079] Alternatively, the composition of structural unit A and structural unit B is not particularly limited and can be appropriately selected taking into consideration antithrombogenicity, durability (the desired degree of immobilization on the plastic fabric substrate), and the like. The composition of structural unit A and structural unit B (structural unit A:structural unit B (molar ratio)) is preferably greater than 1:1 and less than 1:20, more preferably greater than 1:3 and less than 1:20, and particularly preferably 1:4 or greater and less than 1:15. In particular, when the copolymer is a diblock copolymer having a block of structural unit A and a block of structural unit B, the ratio is preferably greater than 1:3 and less than 1:10, more preferably 1:4 or greater and less than 1:7. Such a composition can achieve a good balance between durability (the desired degree of immobilization on the plastic fabric substrate) due to structural unit A and antithrombogenicity due to structural unit B. Furthermore, operability can be further improved (the load during operation can be further reduced). Therefore, antithrombogenicity and operability can be more effectively achieved. The composition of each structural unit is substantially equal to the ratio of the amount (moles) of the monomer charged to the total amount (moles) of the monomers charged when the copolymer is produced.
[0080] The structure of the copolymer according to the present invention is not particularly limited and may be any of a random copolymer, an alternating copolymer, a periodic copolymer, and a block copolymer. Preferably, the copolymer according to the present invention is a random copolymer or a block copolymer. That is, the copolymer according to the present invention is preferably a random copolymer having a segment having structural unit A and a segment having structural unit B, or a block copolymer having a block consisting of structural unit A and a block consisting of structural unit B. More preferably, the copolymer according to the present invention is a random copolymer having a segment having structural unit A and a segment having structural unit B, or a diblock copolymer having a block consisting of structural unit A and a block consisting of structural unit B.
[0081] When the copolymer of the present invention is a random copolymer, it preferably has a hydroxyl group (hydroxyl group (—OH) or carboxyl group (—COOH)) at at least one end, preferably a carboxyl group at at least one end, and preferably a carboxyl group at both ends. In this configuration, the terminal hydroxyl groups (hydroxyl groups and carboxyl groups) of the copolymer do not interact (e.g., due to electrostatic repulsion) with the hydroxyl groups (hydroxyl groups and carboxyl groups) generated on the surface of the plastic fabric substrate by plasma treatment. Therefore, bridging between adjacent fibers (fibers constituting the plastic fabric substrate) can be effectively prevented or suppressed, with one end of the copolymer connecting to one fiber and the other end connecting to an adjacent fiber. That is, in this configuration, the copolymer selectively connects to the surface of a single fiber, allowing a biocompatible layer to be formed on the plastic fabric substrate without filling the gaps between the fibers. Therefore, the biocompatible layer is highly flexible, and medical devices having this configuration have excellent operability (low load during operation). Due to its flexibility, medical devices having the above-described configuration have high conformability to bending and other conditions, allowing them to be easily stored in sheaths or catheters, and are easily pushed out of sheaths or catheters, even around bends, making them easy to place. Furthermore, they are less likely to damage biological tissue (e.g., the inner wall of a biological lumen such as a blood vessel) during placement. In addition, because the spaces between the fibers constituting the plastic fabric substrate are not filled with copolymer, the medical device has excellent permeability. Therefore, for example, when the medical device is an artificial blood vessel, a stent graft, a covered stent, or the like, after placement in the desired biological lumen, endothelial cells can invade not only from the ends of the medical device but also between adjacent fibers, growing and expanding within the lumen of the medical device. Furthermore, the presence of structural unit B provides the biocompatible layer with excellent antithrombotic properties. Because endothelial cells can more quickly coat the inner surface of the medical device and impart antithrombotic properties, improved patency outcomes can be achieved even for medical devices with smaller diameters (e.g., inner diameters of 6 mm or less). Therefore, a medical device having such a configuration can achieve excellent operability as well as excellent antithrombogenicity and antithrombogenicity maintenance (durability) even for medical devices with smaller diameters.It should be noted that the above is merely speculation and does not limit the technical scope of the present invention in any way.
[0082] That is, in a preferred embodiment of the present invention, the copolymer is a random copolymer and has a hydroxyl group or a carboxyl group at at least one end. In a preferred embodiment of the present invention, the copolymer is a random copolymer and has a carboxyl group at at least one end. In a preferred embodiment of the present invention, the copolymer is a random copolymer and has carboxyl groups at both ends.
[0083] Furthermore, when the copolymer is a random copolymer having carboxyl groups at both ends, the carboxyl groups may be derived from the polymerization initiator used when preparing the copolymer. Such a polymerization initiator has a carboxyl group at the end. Examples of such polymerization initiators include 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]tetrahydrate, and 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine)]hydrate. The above polymerization initiators may be used alone or in combination of two or more. That is, in a preferred embodiment of the present invention, when the copolymer is a random copolymer and has a carboxyl group at at least one terminal, the carboxyl group is derived from at least one compound selected from the group consisting of 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]tetrahydrate, and 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]hydrate. In a preferred embodiment of the present invention, when the copolymer is a random copolymer and has carboxyl groups at both terminals, the carboxyl group is derived from 4,4'-azobis(4-cyanovaleric acid) or 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]tetrahydrate. In a preferred embodiment of the present invention, when the copolymer is a random copolymer and has carboxyl groups at least at both ends, the carboxyl groups are derived from 4,4'-azobis(4-cyanovaleric acid).
[0084] Furthermore, when the copolymer of the present invention is a block copolymer, the reactive groups present in the block consisting of structural unit A selectively react with hydroxyl groups (hydroxyl groups and / or carboxyl groups) generated on the surface of the plastic fabric substrate by plasma treatment. Meanwhile, the block consisting of structural unit B does not react with hydroxyl groups generated on the surface of the plastic fabric substrate. Therefore, even in this configuration, bridging between adjacent fibers (fibers constituting the plastic fabric substrate) can be effectively prevented or suppressed, with one end of the copolymer (the block consisting of structural unit A) connecting to one fiber and the other end (the block consisting of structural unit B) connecting to the other adjacent fiber. That is, even in the above configuration, the copolymer selectively connects to the surface of a single fiber, allowing a biocompatible layer to be formed on the plastic fabric substrate without filling the gaps between the fibers. Therefore, the biocompatible layer is highly flexible, and medical devices having this configuration have excellent operability (low load during operation). A medical device having the above configuration exhibits high conformability to bending and other conditions, allowing it to be easily housed in a sheath or catheter, and is easy to push out from the sheath or catheter even around bends, making it easy to place. Furthermore, it is less likely to damage biological tissue (e.g., the inner wall of a biological lumen such as a blood vessel) during placement. In addition, this configuration of the plastic fabric substrate provides excellent permeability because the interfiber spaces are not filled. Therefore, for example, when the medical device is an artificial blood vessel, a stent graft, a covered stent, or a catheter, after placement in the desired biological lumen, endothelial cells can invade not only from the ends of the medical device but also between adjacent fibers, growing and expanding within the lumen of the medical device. The presence of structural unit B provides the biocompatible layer with excellent antithrombotic properties. Because endothelial cells can more quickly coat the inner surface of the medical device and impart antithrombotic properties, it is possible to improve patency outcomes even for medical devices with smaller diameters (e.g., inner diameters of 6 mm or less). Therefore, a medical device having such a configuration can achieve excellent operability as well as excellent antithrombogenicity and antithrombogenicity maintenance (durability) even for medical devices with smaller diameters. Note that the above is speculation and does not limit the technical scope of the present invention in any way.
[0085] That is, in a preferred embodiment of the present invention, it is a block copolymer composed of structural units A and B.
[0086] The copolymer according to the present invention essentially contains the structural unit A and the structural unit B, but may contain other structural units in addition to these structural units. When the copolymer contains other structural units, examples of the other structural units include acrylic acid, methacrylic acid, acryloylmorpholine, N,N-dimethylaminoethyl acrylate, N-vinylpyrrolidone, 2-methacryloyloxyethyl phosphorylcholine, 2-methacryloyloxyethyl-D-glycoside, 2-methacryloyloxyethyl-D-mannoside, vinyl methyl ether, 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, 1-chloro-2-hydroxypropyl (meth)acrylate, and the like. acrylate, 1,6-hexanediol mono(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, neopentyl glycol mono(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolethane di(meth)acrylate, 2-hydroxy-3-phenyloxypropyl(meth)acrylate, 4-hydroxycyclohexyl(meth)acrylate, 2-hydroxy-3-phenyloxy(meth)acrylate, 4-hydroxycyclohexyl(meth)acrylate, cyclohexanedimethanol mono(meth)acrylate, adipic acid, glutaric acid, triethylene glycol, tripropylene glycol, etc. The monomers constituting the other structural units may be used alone or in combination of two or more. That is, the other structural units may be a homopolymer type composed of a single structural unit, or a copolymer type composed of two or more structural units. When two or more types of monomers constituting the other structural units are used, the segment constituted by the monomers may be in the form of a block copolymer, a random copolymer, or an alternating copolymer.
[0087] When the copolymer of the present invention contains other structural units, the content of the other structural units is preferably greater than 0 mol% and less than 5 mol% relative to all structural units constituting the copolymer. That is, when the total of all structural units constituting the copolymer is taken as 100 mol%, the total content of structural units A and B is preferably 95 mol% or more (upper limit: less than 100 mol%). More preferably, the copolymer of the present invention is essentially composed of structural units A and B (content of other structural units = greater than 0 mol% and less than 5 mol%). In this form, the copolymer of the present invention can achieve a good balance between durability (desired degree of immobilization to the plastic fabric substrate) due to structural unit A and antithrombogenicity due to structural unit B. Preferably, the copolymer of the present invention does not contain the other structural units (content of other structural units = 0 mol%).
[0088] The composition of each structural unit (structural units A and B, other structural units) can be measured by a known method. 1 The composition (molar ratio) of the structural units can be determined by measuring the integral ratio of the intensities of each signal in the H-NMR spectrum.
[0089] In one embodiment of the present invention, the copolymer according to the present invention comprises at least one monomer selected from the group consisting of aminomethyl acrylamide, aminomethyl methacrylamide, aminoethyl acrylamide, aminoethyl methacrylamide, aminopropyl acrylamide, aminopropyl methacrylamide (APMA), aminobutyl acrylamide, aminobutyl methacrylamide, and salts thereof, glycidyl acrylate, glycidyl methacrylate (GMA), 3,4-epoxycyclohexylmethyl acrylate, 3,4-epoxycyclohexylmethyl methacrylate, β-methylglycidyl acrylate, and β-methylglycidyl methacrylate. and a structural unit B derived from at least one monomer selected from the group consisting of methoxymethyl acrylate, methoxyethyl acrylate (MEA), ethoxymethyl acrylate, ethoxyethyl acrylate (EEA), 2-(2-ethoxyethoxy)ethyl acrylate (EEEA), tetrahydrofurfuryl acrylate (THFA), methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, 2-(2-ethoxyethoxy)ethyl methacrylate, and tetrahydrofurfuryl methacrylate.
[0090] In one embodiment of the present invention, the copolymer according to the present invention is essentially composed of, or consists of, a structural unit A derived from at least one monomer selected from the group consisting of aminoethyl acrylamide, aminoethyl methacrylamide, aminopropyl acrylamide, aminopropyl methacrylamide (APMA), salts thereof, glycidyl acrylate, and glycidyl methacrylate (GMA), and a structural unit B derived from at least one monomer selected from the group consisting of methoxymethyl acrylate, methoxyethyl acrylate (MEA), methoxypropyl acrylate, ethoxymethyl acrylate, ethoxyethyl acrylate, ethoxypropyl acrylate, ethoxybutyl acrylate, propoxymethyl acrylate, butoxyethyl acrylate, methoxybutyl acrylate, methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, propoxymethyl methacrylate, butoxyethyl methacrylate, and tetrahydrofurfuryl acrylate.
[0091] In one embodiment of the present invention, the copolymer according to the present invention consists essentially of, or consists only of, a structural unit A derived from aminopropyl acrylamide or a salt thereof, aminopropyl methacrylamide (APMA) or a salt thereof, glycidyl acrylate, or glycidyl methacrylate (GMA), and a structural unit B derived from methoxyethyl acrylate and / or tetrahydrofurfuryl acrylate.
[0092] In one embodiment of the present invention, the copolymer according to the present invention consists essentially of, or consists only of, a structural unit A derived from aminopropyl methacrylamide (APMA) or a salt thereof or glycidyl methacrylate (GMA), and a structural unit B derived from methoxyethyl acrylate and / or tetrahydrofurfuryl acrylate.
[0093] In one embodiment of the present invention, the copolymer according to the present invention consists essentially of, or consists only of, a structural unit A derived from aminopropyl methacrylamide (APMA) or a salt thereof or glycidyl methacrylate (GMA), and a structural unit B derived from methoxyethyl acrylate.
[0094] The terminals of the copolymer according to the present invention are not particularly limited and are appropriately determined depending on the type of raw material used, but in one embodiment, they are hydrogen atoms. Furthermore, when the copolymer according to the present invention is prepared by radical polymerization (a radical copolymer), the terminals of the copolymer according to the present invention can be blocked with a structural unit (functional group) derived from a polymerization initiator. When the plastic fabric substrate is a woven fabric, it is preferable that the terminals of the copolymer (radical copolymer) according to the present invention be blocked with a functional group derived from a polymerization initiator, in order to prevent or suppress cross-linking of the copolymer between fibers constituting the substrate.
[0095] The weight-average molecular weight of the copolymer according to the present invention is several thousand to several million, preferably 10,000 to 5 million. In this specification, the "weight-average molecular weight" refers to a value measured by gel permeation chromatography (GPC) using polystyrene as the standard substance and tetrahydrofuran (THF) as the mobile phase. In this specification, the weight-average molecular weight of the copolymer refers to a value measured according to the method described in the Examples. The molecular weight of the copolymer can also be calculated from the type and number of constituent units.
[0096] The thickness (dry film thickness) of the biocompatible layer is, for example, about 0.1 to 10 μm, preferably about 0.5 to 5 μm, and more preferably about 1 to 3 μm.
[0097] The method for producing copolymer is not particularly limited, and can be applied to conventionally known polymerization methods such as radical polymerization, polymerization using macroinitiator, polycondensation method, etc. For example, when each structural unit is arranged randomly (the copolymer is a random copolymer), (i) the method of dissolving monomer A, antithrombotic monomer B and a suitable polymerization initiator, and the monomers constituting other structural units that are added as needed, in a polymerization solvent, and heating the resulting polymerization reaction solution to carry out a polymerization reaction; (ii) the method of dissolving monomer A, antithrombotic monomer B and the monomers constituting other structural units that are added as needed, in a polymerization solvent, and mixing the resulting solution with a separately prepared polymerization initiator solution to prepare a polymerization reaction solution, and carrying out a polymerization reaction.From the viewpoint of ease of operation, method (i) is preferred.
[0098] Here, the polymerization solvent is not particularly limited as long as it can dissolve monomer A, antithrombogenic monomer B, and a suitable polymerization initiator, as well as the monomers constituting other structural units added as needed. Examples of the polymerization solvent include, but are not limited to, one or more selected from water (reverse osmosis water (RO water), pure water, ion-exchanged water, distilled water, etc.); alcohols such as ethanol, isopropanol, n-propanol, n-butanol, isobutanol, sec-butanol, t-butanol, ethylene glycol, diethylene glycol, propylene glycol, and dipropylene glycol; and organic solvents such as chloroform, tetrahydrofuran, acetone, dioxane, and benzene. Furthermore, the concentrations of monomer A and antithrombogenic monomer B contained in the polymerization reaction solution, as well as the monomers constituting other structural units added as needed, are not particularly limited. However, by setting the concentrations relatively high, the weight-average molecular weight of the resulting copolymer can be increased. For example, the concentration (total concentration) of the monomers constituting the monomer A, the antithrombotic monomer B, and other constituent units added as needed in the polymerization reaction solution is preferably 10% by mass or more, more preferably 15% by mass or more. The upper limit of the monomer concentration (total concentration) is not particularly limited, but is, for example, the saturated concentration or less, for example, 70% by mass or less, preferably 50% by mass or less.
[0099] In the polymerization reaction solution, the mixing ratio of the monomer A and the antithrombotic monomer B is preferably adjusted to the above-mentioned preferred composition (molar ratio).
[0100] The polymerization reaction solution may be degassed before the polymerization reaction, for example, by bubbling with an inert gas such as nitrogen gas or argon gas for about 5 minutes to 1 hour.
[0101] The polymerization initiator used here is not particularly limited, and known initiators can be used. Preferably, radical polymerization initiators are used in terms of excellent polymerization stability, and specific examples thereof include persulfates such as potassium persulfate (KPS), sodium persulfate, and ammonium persulfate; peroxides such as hydrogen peroxide, t-butyl peroxide, methyl ethyl ketone peroxide, 3-hydroxy-1,1-dimethylbutyl peroxyneodecanoate, α-cumyl peroxyneodecanoate, 1,1,3,3-tetrabutyl peroxyneodecanoate, t-butyl peroxyneodecanoate, t-butyl peroxyneoheptanoate, t-butyl peroxypivalate, t-amyl peroxyneodecanoate, t-amyl peroxypivalate, di(2-ethylhexyl)peroxydicarbonate, and di(s-butyl)peroxydicarbonate. oxides; azo compounds such as azobisisobutyronitrile (AIBN), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]disulfate dihydrate, 2,2'-azobis(2-methylpropionamidine)dihydrochloride, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine)]hydrate, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine)]tetrahydrate, and azobiscyanovaleric acid. Among these, the polymerization initiator is preferably an azo compound, more preferably an azo compound having a hydroxyl group or a carboxyl group at a terminal, still more preferably 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine)]hydrate, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine)]tetrahydrate, or azobiscyanovaleric acid, and particularly preferably 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine)]tetrahydrate or azobiscyanovaleric acid.The polymerization initiators may be used alone or in combination of two or more.
[0102] Furthermore, for example, the radical polymerization initiator may be combined with a reducing agent such as sodium sulfite, sodium bisulfite, or ascorbic acid to be used as a redox initiator. The amount (addition amount) of the polymerization initiator is preferably 0.01 to 5 mass %, more preferably 0.05 to 3 mass %, relative to 100 mass % of the total of monomer A, antithrombogenic monomer B, and the monomers constituting the other structural units. Alternatively, the amount (addition amount) of the polymerization initiator is preferably 0.1 to 5 mol, more preferably 0.5 to 3 mol, relative to 100 mol of the total of monomer A, antithrombogenic monomer B, and the monomers constituting the other structural units. Such an amount (addition amount) of the polymerization initiator allows for more efficient production of the copolymer.
[0103] When the method (ii) is used, the solvent in which the polymerization initiator is dissolved in advance (the solvent for the polymerization initiator solution) is not particularly limited as long as it can dissolve the polymerization initiator, and examples thereof include the same solvents as the polymerization solvent. The solvent for the polymerization initiator solution may be the same as or different from the polymerization solvent, but is preferably the same solvent as the polymerization solvent in consideration of ease of control of polymerization, etc.
[0104] By heating the polymerization reaction solution prepared as described above, the monomer A, the antithrombotic monomer B, and other monomers constituting the structural units can be copolymerized. Here, as the polymerization method, for example, in addition to the above-mentioned radical polymerization, known polymerization methods such as anionic polymerization and cationic polymerization can be used, but in consideration of ease of operation, radical polymerization is preferably used.
[0105] The polymerization conditions are not particularly limited as long as they allow the polymerization of monomer A, antithrombotic monomer B, and other monomers constituting the structural units. For example, the polymerization temperature is preferably 30 to 150°C, more preferably 40 to 100°C. The polymerization time is preferably 30 minutes to 30 hours, more preferably 1 to 10 hours. Under such conditions, the copolymer can be produced more efficiently.
[0106] During the polymerization, a chain transfer agent, a polymerization rate adjuster, a surfactant, and other additives may be used as needed.
[0107] The environment in which the polymerization reaction is carried out is not particularly limited, and the reaction can be carried out in the air or in an inert gas atmosphere such as nitrogen gas or argon gas, etc. The reaction solution may be stirred during the polymerization reaction.
[0108] After polymerization, the copolymer is preferably purified by a common purification method such as reprecipitation, dialysis, ultrafiltration, or extraction, and particularly preferably by reprecipitation.
[0109] The purified copolymer can be dried by any method, such as freeze-drying, drying under reduced pressure (vacuum drying), spray drying, or heat drying. However, freeze-drying or drying under reduced pressure (vacuum drying) is preferred from the viewpoint of having little effect on the physical properties of the copolymer.
[0110] Furthermore, for example, when the structural units are arranged in blocks (the copolymer is a block copolymer), living radical polymerization or polymerization using a macroinitiator is preferably used. The living radical polymerization method is not particularly limited, but for example, methods described in JP-A-11-263819, JP-A-2002-145971, JP-A-2006-316169, etc., as well as atom transfer radical polymerization (ATRP) methods, etc., can be applied in the same manner or with appropriate modifications. Furthermore, in polymerization methods using a macroinitiator, for example, a copolymer can be prepared by preparing a monomer A having an epoxy group and a macroinitiator having a radically polymerizable group such as a peroxide group, and then polymerizing the macroinitiator with an antithrombotic monomer B in a polymerization solvent.
[0111] The biocompatible layer essentially contains the copolymer of the present invention. The biocompatible layer may contain other components in addition to the copolymer. Examples of other components include unreacted monomers that did not react during polymerization, various additives such as crosslinkers, thickeners, preservatives, and pH adjusters, as well as drugs that suppress vascular stenosis and blockage that may occur when a stent is placed in a lesion. Specific examples of other components include drugs (biologically active substances) such as anticancer drugs, immunosuppressants, antibiotics, antirheumatic drugs, antithrombotic drugs, HMG-CoA reductase inhibitors, ACE inhibitors, calcium channel blockers, antihyperlipidemic drugs, integrin inhibitors, antiallergic drugs, antioxidants, GPIIbIIIa antagonists, retinoids, flavonoids, carotenoids, lipid-improving drugs, DNA synthesis inhibitors, tyrosine kinase inhibitors, antiplatelet drugs, vascular smooth muscle proliferation inhibitors, anti-inflammatory drugs, bio-derived materials, interferons, and NO production promoters. Here, the amounts of other ingredients to be added are not particularly limited, and the amounts normally used are applied in the same manner. Ultimately, the amounts of other ingredients to be added will be appropriately selected by the attending physician in consideration of the severity of the disease to be treated, the patient's weight, etc.
[0112] Preferably, the biocompatible layer is substantially free of other components (i.e., the biocompatible layer is substantially composed of the copolymer of the present invention) (content of other components = less than 10% by mass (solid content), preferably less than 5% by mass (solid content) relative to the mass of the biocompatible layer). More preferably, the biocompatible layer is free of other components (i.e., the biocompatible layer is composed of the copolymer of the present invention).
[0113] [Method for manufacturing a medical device] The method for manufacturing a medical device according to the present invention comprises the steps of plasma treating a plastic fabric substrate to generate hydroxyl groups on the surface of the plastic fabric substrate (step (I)), and then reacting the hydroxyl groups with reactive groups present in the copolymer according to the present invention (step (II)). Each step is described below.
[0114] [Step (I)] In this step, the plastic fabric substrate is plasma-treated. This oxidizes the surface of the plastic fabric substrate, generating hydroxyl groups (hydroxyl groups and carboxyl groups). Here, the plastic fabric substrate is the same as that described in the above section "Plastic Fabric Substrate (Plastic Fabric Substrate Layer)," so a detailed description is omitted here.
[0115] Since the desired plasma treatment can be performed even on a thin and narrow inner surface of a small-diameter artificial blood vessel or the like, the plasma irradiation step is preferably performed by ionized gas plasma treatment.
[0116] Before irradiating the surface of a plastic fabric substrate with ionized gas plasma, it is recommended to clean the surface of the plastic fabric substrate by an appropriate method. That is, it is preferable to remove oils, grease, dirt, etc., adhering to the surface of the plastic fabric substrate before generating hydroxyl groups (-OH) and / or carboxyl groups (-COOH) on the surface of the plastic fabric substrate by ionized gas plasma irradiation. The cleaning method is not particularly limited, and can be performed by cleaning with an appropriate solvent (e.g., ultrasonic cleaning, immersion in a cleaning solvent, or flushing with a cleaning solvent).
[0117] The plasma treatment conditions are not particularly limited. For example, the pressure conditions for the plasma treatment can be either reduced pressure or atmospheric pressure. It is preferable to perform the treatment under atmospheric pressure, because it allows plasma gas to be irradiated from any angle, the apparatus can be made smaller because a vacuum device is not required, a space-saving and low-cost system configuration can be realized, and it is also economically advantageous. Furthermore, by irradiating the plasma gas while rotating the plasma irradiation nozzle around the object to be treated, such as an artificial blood vessel, the entire circumference of the object to be treated can be uniformly plasma-treated without unevenness.
[0118] The ionized gas that can be used in the plasma treatment is one or more gases selected from the group consisting of helium, neon, argon, krypton, air, oxygen, carbon dioxide, carbon monoxide, water vapor, nitrogen, hydrogen, etc. The plasma treatment conditions (irradiation time, LF output, applied current, gas flow rate, electrode gap, plasma irradiation distance) are not particularly limited and can be appropriately selected depending on the bonding strength (ease of immobilization) between the copolymer and the plastic cloth substrate, the type and area of the plastic cloth substrate used, etc.
[0119] For example, the irradiation time in the plasma treatment is preferably more than 10 seconds, more preferably 30 seconds to 10 minutes, and particularly preferably 1 to 5 minutes, which allows the copolymer to be more firmly supported (fixed) on the surface of the plastic cloth substrate layer.
[0120] As an example, the LF output in the plasma treatment is preferably 100 to 300 W, and more preferably 200 W.
[0121] As an example, the gas flow rate in plasma processing is 5 to 20 cm 3 / min, and preferably 15 cm 3 / min is more preferable.
[0122] The temperature of the object to be treated (plastic fabric substrate) in the plasma treatment is not particularly limited as long as it is lower than the melting point of the plastic (polymer) on the substrate surface and does not deform the plastic fabric substrate, and may be room temperature or may be heated or cooled. From an economical point of view, it is preferable to perform the treatment at a temperature (e.g., 5 to 35°C) that does not require a heating or cooling device.
[0123] Plasma irradiation devices (systems) that can be used for plasma treatment are not particularly limited, and examples include plasma irradiation devices (systems) configured to include a plasma generating tube that introduces gas molecules and excites them to generate plasma, and an electrode that excites the gas molecules in the plasma generating tube, and to emit plasma from one end of the plasma generating tube. However, the present invention is not limited to such configurations (systems). Examples include devices that employ a high-frequency induction system, a capacitively coupled electrode system, a corona discharge electrode-plasma jet system, a parallel plate system, a remote plasma system, an atmospheric pressure plasma system, a low-pressure plasma system, an ICP high-density plasma system, and the like. Additionally, commercially available ionized gas plasma irradiation devices (systems), particularly atmospheric pressure plasma irradiation devices (systems), suitable for irradiation of artificial blood vessels, stent grafts, covered stents, and the like, can be used. Specifically, a plasma irradiation device such as DURADYNE (product name or trademark) manufactured by TRI-STAR TECHNOLOGIES or a plasma irradiation device such as PLASMABEAM manufactured by DIENER ELECTRONIC can be used, but the present invention is not limited to these.
[0124] [Step (II)] In this step, the hydroxyl groups (-OH, -COOH) generated on the surface of the plastic fabric substrate in step (I) react with reactive groups present in the copolymer of the present invention to form chemical bonds. Because this reaction occurs on the surface of the fibers that make up the plastic fabric substrate, the copolymer of the present invention can be selectively immobilized on the surface of the fibers that make up the plastic fabric substrate. In particular, when the copolymer is a random copolymer having a carboxyl group at at least one end or a block copolymer composed of structural units A and B, the end of the copolymer does not interact with the hydroxyl groups (-OH, -COOH) on the plastic fabric substrate. Therefore, the copolymer is selectively immobilized on the surface of the fibers that make up the plastic fabric substrate without bridging between adjacent fibers.
[0125] That is, the present invention also provides a medical device comprising a plastic fabric substrate and a biocompatible layer supported on at least a portion of the plastic fabric substrate, wherein the biocompatible layer comprises a copolymer having a structural unit A derived from a monomer having a reactive group that reacts with a hydroxyl group in its molecule and a structural unit B derived from a (meth)acrylic acid ester represented by formula (I), and the substrate layer is bonded to the biocompatible layer (bonded to the biocompatible layer via the reactive group). In this embodiment, the copolymer is selectively immobilized on the surfaces of the fibers that make up the plastic fabric substrate without bridging between adjacent fibers that make up the plastic fabric substrate.
[0126] The medical device obtained by the above method or the medical device having the above configuration (the medical device of the present invention) is highly flexible and has excellent operability (the load during operation can be kept low). Furthermore, the flexibility of the medical device of the present invention allows it to easily conform to bending and other conditions. Therefore, it can be easily stored in a sheath or catheter, and the medical device can be easily pushed out of the sheath or catheter even around bent sections, making it easy to place. Furthermore, it is less likely to damage biological tissue (e.g., the inner wall of a biological lumen such as a blood vessel) during placement. In addition, since the spaces between the fibers constituting the plastic fabric substrate are not filled with copolymer, the medical device has excellent permeability. Therefore, for example, when the medical device is an artificial blood vessel, a stent graft, a covered stent, or the like, after placement in the desired biological lumen, endothelial cells can invade not only from the ends of the medical device but also between adjacent fibers, allowing them to rapidly grow and expand within the lumen of the medical device. Furthermore, the presence of structural unit B provides the biocompatible layer with excellent antithrombogenicity. Because endothelial cells can more quickly coat the inner surface of a medical device and impart antithrombogenicity, it is possible to improve the patency outcome even for smaller-diameter medical devices. Therefore, a medical device having such a configuration can achieve not only excellent operability but also excellent antithrombogenicity and antithrombogenicity maintenance (durability) even for smaller-diameter medical devices. Note that the above is speculation and does not in any way limit the technical scope of the present invention.
[0127] Here, the copolymer is the same as that explained in the section "Biocompatible Layer (Antithrombogenic Layer)" above, and therefore, explanation thereof will be omitted here.
[0128] The reaction method is not particularly limited, but may be, for example, by contacting at least a portion of a plastic fabric substrate with the copolymer (preferably by applying a coating solution containing the copolymer). Here, "contacting at least a portion of a plastic fabric substrate with the copolymer" refers to bringing at least a portion of the plastic fabric substrate and the copolymer (which may be in the form of a solution containing the copolymer or a composition containing the copolymer) close enough to react, interact, or physically contact each other. Examples of the "interaction" include, but are not limited to, chemical bonds such as covalent bonds, coordinate bonds, ionic bonds, hydrogen bonds, and van der Waals bonds.
[0129] A preferred form of "contact" is contact by application, i.e., the method for producing a medical device according to the present invention preferably comprises applying a solution (coating liquid) containing a copolymer and a solvent to at least a portion of a plastic fabric substrate to form a biocompatible layer.
[0130] The above embodiment will be described below, but the present invention is not limited to the following embodiment.
[0131] A solution containing the copolymer, a solvent, and, if necessary, other components (also referred to simply as a "coating solution" in this specification) is prepared, and the coating solution is applied to a plastic fabric substrate to form a coating film on the substrate. The method for preparing and applying the coating solution is not particularly limited except for using a solution containing the copolymer and a solvent, and can be applied in the same manner as a known method or by appropriately modifying it.
[0132] The solvent used to prepare the coating liquid is not particularly limited and is appropriately selected depending on the type of copolymer (and other components, if used). From the viewpoint of high solubility, water (reverse osmosis water (RO water), pure water, ion-exchanged water, distilled water, etc.); alcoholic solvents such as methanol, ethanol, isopropyl alcohol, and butanol; and organic solvents such as dichloromethane, chloroform, carbon tetrachloride, tetrahydrofuran (THF), dimethyl sulfoxide, N,N-dimethylformamide (DMF), acetone, dioxane, and benzene are preferably used. These solvents may be used alone or in combination of two or more (in the form of a mixed solvent).
[0133] The concentration of the copolymer in the coating solution is not particularly limited. For example, the concentration of the copolymer in the coating solution is preferably 0.01 to 10% by mass, more preferably 0.05 to 5% by mass, and particularly preferably 0.1 to 1% by mass. When the copolymer concentration is within the above range, the resulting biocompatible layer can fully exhibit the effects of the present invention. Furthermore, a uniform biocompatible layer of the desired thickness can be easily obtained with a single coating, and the viscosity of the solution falls within an appropriate range, which is preferable in terms of operability (e.g., ease of coating) and production efficiency. However, concentrations outside the above range are also fully usable as long as they do not affect the effects of the present invention.
[0134] The coating liquid may contain other components in addition to the copolymer and the solvent. Here, the other components include a dehydration condensation agent in addition to the other components described above. In particular, when the copolymer contains a primary amino group (-NH 2), it is preferable that the coating liquid further contains a dehydrating condensation agent. The dehydrating condensation agent can further promote the reaction between the reactive groups of the copolymer and the hydroxyl groups (particularly carboxyl groups) generated on the surface of the plastic fabric substrate. The dehydrating condensation agent is not particularly limited as long as it is water-soluble and capable of reacting with carboxyl groups (-COOH) or hydroxyl groups (-OH) in an aqueous solution. Specific examples include triazine-based condensation agents such as 4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride (DMT-MM), a water-soluble salt of 1-cyclohexyl-3-(2-morpholinoethyl)carbodiimide, and 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride (WSC).
[0135] When the coating solution further contains a dehydrating condensation agent, the amount of the dehydrating condensation agent in the coating solution is not particularly limited, but it is preferable that the agent be present in excess relative to the copolymer. For example, the dehydrating condensation agent in the coating solution is present in an amount greater than 1 mole and less than 5 moles, preferably 1.5 to 5 moles, and more preferably 2 to 4 moles, per mole of copolymer. When the amount of the dehydrating condensation agent is within the above range, the primary amino groups of the copolymer can react more efficiently with the hydroxyl groups (especially carboxyl groups) generated on the surface of the plastic fabric substrate. The dehydrating condensation agent may be used alone or in combination of two or more types.
[0136] Next, the coating solution prepared as described above is applied onto a plastic fabric substrate.
[0137] The method for applying (coating) the coating liquid to the surface of the plastic fabric substrate is not particularly limited, and conventionally known methods can be applied, such as coating / printing, immersion (dipping, dip coating), spraying, spin coating, mixed solution impregnated sponge coating, bar coating (e.g., wire bar), die coating, reverse coating, comma coating, gravure coating, doctor knife, etc. Of these, immersion (dipping, dip coating) and bar coating are preferred, with immersion being more preferred.
[0138] When forming a biocompatible layer on a narrow inner surface of an artificial blood vessel, a stent graft, a covered stent, etc., a plastic fabric substrate may be immersed in the coating solution and degassed by reducing the pressure in the system. By reducing the pressure and degassing, the solution can be rapidly penetrated into the narrow inner surface, facilitating the formation of a biocompatible layer.
[0139] Alternatively, the application (coating) may be performed while stirring the coating liquid. This further promotes contact of the coating liquid with the workpiece, such as an artificial blood vessel. The stirring can be performed using a known device such as an orbital shaker, rotary shaker, or paint shaker. The stirring conditions are not particularly limited. From the viewpoint of more efficient contact with the workpiece, such as an artificial blood vessel, the stirring speed is, for example, 200 to 700 rpm. From the same viewpoint, the stirring time is, for example, 1 to 5 hours. The stirring temperature may be around room temperature (e.g., 20 to 40°C), but heating may be used as long as it is lower than the boiling point of the solvent used.
[0140] Furthermore, when forming a biocompatible layer only on a portion of a plastic cloth substrate, the biocompatible layer can be formed on the desired surface area of the substrate by immersing only a portion of the plastic cloth substrate in a coating liquid and coating the coating liquid onto that portion of the plastic cloth substrate.
[0141] If it is difficult to immerse only a portion of the plastic fabric substrate in the coating solution, the surface portion of the substrate that does not require the formation of a biocompatible layer can be protected (e.g., coated) with a suitable removable member or material. The substrate can then be immersed in the coating solution to coat the plastic fabric substrate with the coating solution. The protective member (material) covering the surface portion of the substrate that does not require the formation of a biocompatible layer can then be removed, and the substrate can then be reacted by heating or other means to form a biocompatible layer on the desired surface portion of the substrate. However, the present invention is not limited to these formation methods, and any conventionally known method can be used to form a biocompatible layer. For example, if it is difficult to immerse only a portion of the plastic fabric substrate in the coating solution, other coating techniques (e.g., applying the coating solution to a desired surface portion of a medical device using an applicator such as a sprayer, bar coater, die coater, reverse coater, comma coater, gravure coater, spray coater, or doctor knife) can be used instead of the immersion method. In addition, when the structure of a cylindrical medical device requires that both the outer and inner surfaces of the device have a biocompatible layer, the immersion method (dipping method) is preferably used because it allows both the outer and inner surfaces to be coated at the same time.
[0142] The amount of coating liquid to be applied is preferably selected so that the thickness (dry film thickness) of the resulting biocompatible layer falls within the above range.
[0143] The biocompatible layer formed as described above is then dried, if necessary, to form a biocompatible layer on the plastic fabric substrate. This allows the reactive groups contained in the copolymer to react with the surface of the plastic fabric substrate (the hydroxyl and / or carboxyl groups formed by the plasma irradiation process) to support (immobilize) the biocompatible layer on the plastic fabric substrate. Furthermore, the reactive groups (especially epoxy groups) of the copolymer react with each other to increase the film strength of the biocompatible layer.
[0144] Drying treatments include natural drying, air drying, or heat treatment. Natural drying or air drying is particularly preferred when using a plastic fabric substrate with low heat resistance. Furthermore, when heat treatment is performed, the conditions for the heat treatment are not particularly limited as long as they allow the solvent to be removed (i.e., a biocompatible layer can be formed on the plastic fabric substrate), and can be appropriately selected depending on the type of solvent. For example, the heat treatment temperature is preferably 40 to 150°C. The heat treatment time is preferably 30 minutes to 30 hours. Under these conditions, the epoxy groups of the copolymer in the coating layer can react more effectively with the surface of the plastic fabric substrate (preferably the hydroxyl and / or carboxyl groups formed by the plasma irradiation process), thereby more firmly immobilizing the copolymer to the plastic fabric substrate. Furthermore, the epoxy groups of the copolymer in the coating layer can react more efficiently with each other, further increasing the film strength of the biocompatible layer. Therefore, a high-strength biocompatible layer that does not easily peel off from the plastic fabric substrate can be formed.
[0145] The pressure conditions in the drying step are not particularly limited, and the drying step may be carried out under normal pressure (atmospheric pressure), or may be under increased or reduced pressure. As a drying (or heating) means (apparatus), for example, an oven or a reduced-pressure dryer can be used, but in the case of natural drying, no particular drying means (apparatus) is required.
[0146] In this step, the biocompatible layer may be washed if necessary. The washing method is not particularly limited, but may include immersing the biocompatible layer in a washing solvent, pouring the washing solvent over the biocompatible layer, or a combination of these. The washing solvent used is not particularly limited as long as it does not dissolve the biocompatible layer. Water (e.g., ion-exchanged water, distilled water, RO water, filtered water, sterilized water, purified water, etc.) or warm water is preferably used. The temperature of the washing water is not particularly limited, but is preferably 20°C to 80°C. The washing time (the time the washing solvent is in contact with the biocompatible layer) is not particularly limited, but is preferably 1 to 60 minutes. After the washing step, a drying step may be further performed. The drying method and drying conditions (temperature, time, etc.) are not particularly limited, and conventionally known methods can be used.
[0147] The above method allows the production of a medical device that is both antithrombogenic and easy to handle (low load during operation), and also allows the production of a medical device that is excellent in at least one of antithrombogenicity and durability (ability to maintain antithrombogenicity for a longer period of time).
[0148] [Uses of Medical Devices] The medical device according to the present invention has excellent antithrombotic properties. Examples of medical devices according to the present invention include implantable artificial organs and treatment instruments, extracorporeal circulation artificial organs, catheters, guide wires, etc. Among these, the medical device is preferably an intravascular device, and specific examples include artificial blood vessels, stents, stent grafts, covered stents, artificial valves, valve clips, and auxiliary circulation pump catheters. The medical device according to one embodiment of the present invention is an artificial blood vessel, a stent graft, a covered stent, or a catheter. Other examples of medical devices include the following: Specific examples include implantable medical devices such as artificial trachea, artificial skin, and artificial pericardium; artificial organ systems such as artificial heart systems, artificial lung systems, artificial heart-lung systems, artificial kidney systems, artificial liver systems, and immunoregulatory systems; catheters inserted or placed in blood vessels such as indwelling needles, IVH catheters, drug administration catheters, thermodilution catheters, angiography catheters, vasodilator catheters, dilators, and introducers; guide wires and stylets for these catheters; and catheters inserted or placed in biological tissues other than blood vessels, such as gastric catheters, nutrition catheters, enteral feeding (ED) tubes, urethral catheters, urinary catheters, balloon catheters, and various suction catheters and drainage catheters, including endotracheal suction catheters.
[0149] The effects of the present invention will be explained using the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. In the following examples, unless otherwise specified, operations were performed at room temperature (25°C). Furthermore, unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.
[0150] The weight average molecular weight (Mw) of the copolymer was measured according to the following method.
[0151] (Measurement of Weight Average Molecular Weight) In this specification, the "weight average molecular weight" refers to a value measured by gel permeation chromatography (GPC) using polystyrene as a standard substance and tetrahydrofuran (THF) as a mobile phase. Specifically, a polymer (copolymer) is dissolved in tetrahydrofuran (THF) to a concentration of 10 mg / mL to prepare a sample. For the sample prepared in this manner, a GPC column LF-804 (manufactured by Shodex) is attached to a GPC system LC-20 (manufactured by Shimadzu Corporation), THF is run as the mobile phase, and polystyrene is used as a standard substance to measure the GPC of the copolymer (polymer). After preparing a calibration curve using standard polystyrene, the weight average molecular weight of the copolymer (polymer) is calculated based on this curve.
[0152] Example 1 1. Synthesis of MEA-APMA random copolymer [P(MEA-r-APMA(14 / 1))] 1-1. Set-up A water bath was filled with tap water, and the water surface was covered with a polypropylene (PP) ball. Next, the water bath was placed on a magnetic stirrer, and the temperature was set to 80°C.
[0153] 1-2. Polymerization of P(MEA-r-APMA) To a 250 mL three-neck flask were added 2.00 g (11 mmol) of N-(3-aminopropylmethacrylamide) hydrochloride (APMA) (manufactured by Combi-Blocks), 20.24 g (156 mmol) of 2-methoxyethyl acrylate (MEA), 0.44 g (1.6 mmol) of 4,4′-azobis(4-cyanovaleric acid) (ACVA) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a polymerization initiator, as well as approximately 30 mL of 1,4-dioxane and approximately 20 mL of RO water.
[0154] A stirrer was placed in the three-neck flask, and the mixture was stirred at room temperature (25°C) until all the reagents were dissolved. Nitrogen bubbling was performed from the end of the three-neck flask for approximately 30 minutes. A cooling tube was placed in the center of the three-neck flask, and cooling water at room temperature (approximately 15 to 25°C) was poured into it. A thermocouple was inserted into the remaining neck of the three-neck flask to record the solution temperature during the reaction. The three-neck flask was immersed in a water bath set to 80°C, and the reaction was carried out for approximately 3 hours. After the reaction time, the three-neck flask was removed from the water bath and cooled to room temperature (25°C). This yielded a reaction solution containing P(MEA-r-APMA).
[0155] 1-3. Purification of P(MEA-r-APMA) 250 mL each of hexane and isopropyl alcohol (IPA) was added to a 1-L beaker. The reaction solution obtained in 1-2 above was poured into this 1-L beaker, stirred for 15 minutes, and the supernatant was gently removed. The precipitated polymer was dissolved in a 4:1 (v / v) tetrahydrofuran (THF)-ethanol mixed solution (THF = 40 mL, ethanol = 10 mL) (Polymer Solution 1). A 70:30 (v / v) hexane-IPA solution (hexane = 350 mL, IPA = 150 mL) was further added to this polymer solution 1, and the mixture was stirred for 15 minutes to precipitate the polymer. The supernatant was then gently removed. The precipitated polymer was again dissolved in a 4:1 (v / v) tetrahydrofuran (THF)-ethanol mixed solution (THF = 40 mL, ethanol = 10 mL) (Polymer Solution 2). Furthermore, 500 mL of hexane was added to this polymer solution 2, and the mixture was stirred for 20 minutes to precipitate the polymer, after which the supernatant was gently removed. The precipitated polymer was dissolved in a small amount (approximately 30 mL) of ethanol and transferred to a plastic cup. The plastic cup was placed in a draft chamber, and the solvent was thoroughly evaporated in the draft chamber. The mixture was then vacuumed at room temperature (25°C) for 20 hours to dry the polymer. This yielded an MEA-APMA random copolymer (MEA:APMA = 14:1 (molar ratio)) [P(MEA-r-APMA)].
[0156] 2. Preparation of sample (1): P(MEA-r-APMA) bonding to PET woven fabric using DMT-MM 2-1. Preparation of plastic fabric substrate The woven fabric alone was removed from a cylindrical polyethylene terephthalate (PET) woven fabric (diameter: 8 mm, length: 13 cm, thickness: 0.15 mm) with a stent sewn onto it, to a size of 1 cm x 1 cm (1 cm 2 The cloth was cut into pieces of cloth measuring 100 mm in diameter, immersed in ethanol for 1 minute, and then the ethanol was discarded. This procedure was repeated three times to perform washing (PET woven fabric 1).
[0157] The above-mentioned washed PET woven fabric 1 was set in a plasma irradiation device (low-pressure plasma type) and plasma was irradiated on both sides for 3 minutes under the conditions described below. After plasma irradiation, the PET woven fabric was taken out into the atmosphere and allowed to stand for 30 minutes, thereby generating hydroxyl groups (—OH) and carboxyl groups (—COOH) on the surface of the PET woven fabric 1 (PET woven fabric 2).
[0158] (Plasma irradiation conditions) Apparatus: manufactured by Diener Electronic, product name: Pico Introduced gas: argon gas (100% by volume) Pressure: 0.3 mbar Power: 50% LF output: 200 W Gas flow rate: 15 sccm Treatment time: 3 minutes.
[0159] 2-2. Bonding of P(MEA-r-APMA) to PET Woven Fabric 2 (Plastic Fabric Substrate) 624 mg (2.25 mmol) of 4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride (DMT-MM) (dehydration condensation agent) was dissolved in a small amount (1 mL) of RO water to prepare a DMT-MM solution.
[0160] 100 mg (0.75 mmol) of P(MEA-r-APMA) obtained in 1-3 above was dissolved in 10 mL of RO water to prepare a P(MEA-r-APMA) solution. This P(MEA-r-APMA) solution was transferred to a 50 mL Falcon (registered trademark, the same applies hereinafter) tube.
[0161] The PET woven fabric (PET woven fabric 2) irradiated with plasma in 2-1 above was placed in a Falcon tube containing the P(MEA-r-APMA) solution and stirred for 3 hours at 400 rpm with an orbital shaker (Nisshin Rika Co., Ltd., Rotary Shaker NX-20). After stirring for the predetermined time, 1 mL of the DMT-MM solution was added to the Falcon tube. Immediately after the dropwise addition was completed, stirring of the Falcon tube with the orbital shaker was started and stirred for 3 hours at 400 rpm. After stirring for the predetermined time, the Falcon tube was removed from the orbital shaker and allowed to stand at room temperature overnight to confirm the decomposition of the primary amino group (-NH 2 ) was reacted with carboxyl or hydroxyl groups on the surface of PET woven fabric 2 (plastic fabric substrate) (PET woven fabric 3).
[0162] The PET woven fabric 3 was removed from the Falcon tube and immersed in 50 mL of RO water for 5 minutes, after which the RO water was replaced with fresh water for cleaning (cleaning operation). This cleaning operation was then repeated three times (PET woven fabric 4), after which the PET woven fabric 4 was removed from the RO water and allowed to dry at room temperature to obtain sample (1) in which P(MEA-r-APMA) (biocompatible layer) was immobilized on the PET woven fabric.
[0163] The surface of Sample (1) of Example 1 was observed with a scanning electron microscope (SEM). The results are shown in Figure 3. Figures 3A and 3B show SEM images at 200x and 1000x magnifications, respectively. Figure 3 shows that in Sample (1), P(MEA-r-APMA) can be selectively immobilized on the surface of a single fiber of the PET woven fabric without bridging between the fibers. This is presumably because P(MEA-r-APMA) has carboxyl groups derived from 4,4'-azobis(4-cyanovaleric acid) (a polymerization initiator) at both ends, and these carboxyl groups at both ends electrostatically repel the carboxyl and hydroxyl groups generated on the PET woven fabric by plasma irradiation.
[0164] Furthermore, the antithrombotic properties of sample (1) were evaluated by a platelet adhesion test according to the following method.
[0165] (Antithrombotic Evaluation Method) Anticoagulated fresh porcine blood (1) was obtained by adding 3.2 (w / v)% sodium citrate (anticoagulant) aqueous solution to fresh porcine blood. The volume ratio of fresh porcine blood to sodium citrate was 9:1. A 1M calcium chloride solution and a 1000 U / mL heparin solution were dispensed into a 15 mL Falcon tube to prepare a mixed solution. This mixed solution was added to the anticoagulated fresh porcine blood (1) and stirred slowly to avoid foaming, to obtain anticoagulated fresh porcine blood (2). The mixture was adjusted so that 820 μL of the 1M calcium chloride solution and 100 μL (100 U) of the 1000 U / mL heparin solution were contained in 50 mL of anticoagulated fresh porcine blood (2). The final concentration of heparin in the anticoagulated fresh porcine blood (2) was 2.0 U / mL. 100 μL of anticoagulated fresh porcine blood (2) was centrifuged (1500 × g) at 22°C for 10 minutes to obtain platelet-rich plasma (PRP). This PRP was poured into cylindrical containers with the above samples attached to their bottoms and allowed to stand at room temperature for 5 hours. Each sample was then washed with a 3.2 wt% sodium citrate / phosphate buffer solution (PBS) (= 1 / 9) and fixed with a 1 (w / v)% glutaraldehyde PBS solution. After standing overnight in a refrigerator (4°C), the glutaraldehyde PBS solution was removed using a pipette tube and washed seven times with RO water. Each sample was allowed to stand at room temperature and dried. The dried samples were fixed to stainless steel plates, platinum-deposited by platinum sputtering, and then observed and photographed (1000x magnification) using a scanning electron microscope (SEM). The results are shown in Figure 4A. Figure 4A shows that almost no platelet adhesion was observed on the surface of Sample (1) of Example 1. From this, it is considered that in Sample (1) of Example 1, P(MEA-r-APMA), which has excellent antithrombotic properties, is sufficiently immobilized on the fiber surface of the PET woven fabric.
[0166] Furthermore, for Sample (1) of Example 1, the operability was evaluated using a force gauge according to the following method. Each evaluation was performed in triplicate, and the insertion load and its average value for each sample (dry and wet) are shown in Table 1 (evaluation of dry samples) and Table 2 (evaluation of wet samples), respectively.
[0167] (Method for evaluating operability using a force gauge (evaluation of a dry sample)) In order to confirm that the physical properties of the stent graft are not affected, the load required to pull a dry sample into a tube simulating a sheath was measured according to the method below.
[0168] A dry sample (1-1) was prepared in the same manner as sample (1) used in the platelet adhesion test, except that a cylindrical polyethylene terephthalate (PET) woven fabric (diameter: 8 mm, length: 13 cm, thickness: 0.15 mm) with a stent sewn onto it was cut into a 3 cm-long cylindrical piece so that the sewn stent remained.
[0169] The dry sample (1-1) obtained above was further cut into a 1 cm long tube so that the sewn stent remained, and three holes were made at the tip with tweezers, and a piece of fishing line was passed through each hole. The fishing line was hooked onto the hook of a force gauge, and using a funnel-shaped jig with a narrow diameter part of about 5 mm, the load (gf) applied when the sample was pulled from the funnel part to the narrow diameter part was measured with the force gauge.
[0170] (Method for evaluating operability using a force gauge (evaluation of a wet sample)) In order to confirm that the physical properties of the stent graft are not affected, the load required to pull a wet sample into a tube simulating a sheath was measured according to the method described below.
[0171] Dry samples (1-1) were prepared in the same manner as described above (Method for evaluating operability using a force gauge (evaluation of dry samples)). Each sample (1-1) was cut into a 1 cm long cylinder, and three holes were made at the tip with tweezers, and a string was passed through each hole. This was immersed in RO water at room temperature for 10 minutes to prepare a wet sample. The string was hooked onto the hook of a force gauge, and a funnel-shaped jig with a diameter of the narrow part of about 5 mm was used to measure the load (gf) applied when the sample was pulled from the funnel part to the narrow part with the force gauge.
[0172] Example 2 1. Synthesis of MEA-GMA Block Copolymer [P(MEA-b-GMA)(10 / 1)] 29.7 g of triethylene glycol was added dropwise to 72.3 g of adipic acid dichloride at 50°C, and then the hydrochloric acid was removed under reduced pressure at 50°C for 3 hours to obtain an oligoester. Next, 4.5 g of methyl ethyl ketone was added to 22.5 g of the obtained oligoester, and this was added dropwise to a solution consisting of 5 g of sodium hydroxide, 6.93 g of 31% hydrogen peroxide, 0.44 g of dioctyl phosphate as a surfactant, and 120 g of water, and the mixture was allowed to react at -5°C for 20 minutes. The obtained product was repeatedly washed with water and methanol and then dried to obtain a polyperoxide (PPO) having multiple peroxide groups in the molecule. Next, 0.5 g of this PPO, 9.5 g of glycidyl methacrylate (GMA), and benzene as a solvent were polymerized at 65°C for 2 hours under reduced pressure with stirring. The reaction product obtained after polymerization was reprecipitated with diethyl ether to obtain polyGMA (PPO-GMA) having peroxide groups in the molecule. Next, 0.225 g of the obtained PPO-GMA (equivalent to 0.00165 mol of GMA) was used as a polymerization initiator, and 2.16 g (0.01665 mol) of methoxyethyl acrylate (2-MTA, manufactured by Osaka Organic Chemical Industry Co., Ltd.) was dissolved in 1,4-dioxane, and polymerization was carried out at 80°C for 5 hours under a nitrogen atmosphere. The reaction product obtained after polymerization was reprecipitated with hexane and recovered to obtain a block copolymer (MEA:GMA = 10:1 (molar ratio)) (P(MEA-b-GMA)1) having methoxyethyl acrylate and glycidyl methacrylate as structural units.
[0173] 2. Preparation of Sample (2): Bonding of P(MEA-b-GMA)1 to PET Woven Fabric 2-1. Preparation of Plastic Fabric Substrate PET woven fabric 2 was prepared in the same manner as in Example 1.
[0174] 2-2. Bonding of P(MEA-b-GMA)1 to PET woven fabric 2 (plastic fabric substrate) The glycidyl group (—CH 2 -C 2 H 3 O) was reacted with the hydroxyl or carboxyl groups on the surface of a PET woven fabric 2 (plastic fabric substrate), and a sample (2) was prepared in which P(MEA-b-GMA)1 (biocompatible layer) was immobilized on the PET woven fabric 2.
[0175] Polymer solution 1 was prepared by dissolving 100 mg of the P(MEA-b-GMA)1 obtained above in 20 mL of a mixed solvent (RO water:methanol:acetone=2:3:5 (volume ratio)).
[0176] The polymer solution 1 prepared above was transferred to a recovery flask and nitrogen was bubbled through it for 5 minutes (polymer solution 2).
[0177] The PET woven fabric 2 (plasma-irradiated PET substrate) prepared in 2-1 above was placed into the polymer solution 2, and nitrogen bubbling was continued for an additional 5 minutes. The opening of the recovery flask was sealed with a rubber stopper, and the mixture was allowed to react for 4 hours in a water bath set at 37°C, resulting in immobilization of P(MEA-b-GMA)1 (biocompatible layer) on the PET woven fabric 2 (immobilized PET woven fabric). After the reaction time, the immobilized PET woven fabric was removed from the recovery flask and stirred in ethanol for 1 hour to remove unreacted copolymer (washed PET woven fabric). After 1 hour, the washed PET woven fabric was removed from the ethanol and air-dried in a fume hood to obtain sample (2) in which P(MEA-b-GMA)1 (biocompatible layer) was immobilized on the PET woven fabric.
[0178] The surface of Sample (2) of Example 2 was observed with a scanning electron microscope (SEM). The results are shown in Figure 3. Figures 3C and 3D show SEM images at 200x and 1000x magnifications, respectively. Figure 3 shows that in Sample (2), P(MEA-b-GMA)1 can be selectively immobilized on the surface of a single fiber of the PET woven fabric without bridging between fibers. This is presumably because the P(MEA-b-GMA)1 terminal does not interact with the carboxyl or hydroxyl groups formed on the PET woven fabric.
[0179] Furthermore, the antithrombogenicity of Sample (2) of Example 2 was evaluated by a platelet adhesion test in the same manner as in Example 1. The results are shown in FIG. 4B. From FIG. 4B, almost no platelet adhesion was observed on the surface of Sample (2) of Example 2. From this, it is considered that Sample (2) of Example 2 has P(MEA-b-GMA)1, which has excellent antithrombogenicity, sufficiently immobilized on the fiber surface of the PET woven fabric.
[0180] In addition, a cylindrical polyethylene terephthalate (PET) woven fabric (diameter: 8 mm, length: 13 cm, thickness: 0.15 mm) with a stent sewn onto it was cut into a 3 cm cylindrical shape so that the sewn stent remained, and Sample (2-1) was prepared in the same manner as Sample (2), except that Sample (2-1) was used. The operability was evaluated using a force gauge in the same manner as in Example 1. The results are shown in Tables 1 and 2 below.
[0181] Example 3 1. Synthesis of MEA-GMA Block Copolymer [P(MEA-b-GMA)(7 / 1)] PolyGMA (PPO-GMA) having peroxide groups in the molecule was obtained in the same manner as in Example 2. Subsequently, 0.33 g of the obtained PPO-GMA (corresponding to 0.00225 mol of GMA) was used as a polymerization initiator to dissolve 2.025 g (0.0156 mol) of methoxyethyl acrylate (2-MTA, manufactured by Osaka Organic Chemical Industry, Ltd.) in 1,4-dioxane, and the resulting solution was polymerized at 80°C for 5 hours under a nitrogen atmosphere. The reaction product obtained after polymerization was reprecipitated with hexane and recovered to obtain a block copolymer (MEA:GMA = 7:1 (molar ratio)) (P(MEA-b-GMA)2) composed of methoxyethyl acrylate and glycidyl methacrylate as structural units.
[0182] 2. Preparation of Sample (3): Bonding of P(MEA-b-GMA)2 to PET Woven Fabric Sample (3) was prepared in the same manner as in Example 2, except that the P(MEA-b-GMA)2 obtained above was used instead of P(MEA-b-GMA)1 in Example 2. The glycidyl groups of P(MEA-b-GMA)2 were reacted with the hydroxyl or carboxyl groups on the surface of PET woven fabric 2 (plastic fabric substrate), thereby immobilizing P(MEA-b-GMA)2 (biocompatible layer) on PET woven fabric 2.
[0183] The surface of Sample (3) of Example 3 was observed with a scanning electron microscope (SEM). The results are shown in Figure 3. Figures 3E and 3F show SEM images at 200x and 1000x magnifications, respectively. Figure 3 shows that in Sample (3), P(MEA-b-GMA)2 can be selectively immobilized on the surface of a single fiber of the PET woven fabric without bridging between fibers. This is presumably because the P(MEA-b-GMA)2 terminal does not interact with the carboxyl or hydroxyl groups formed on the PET woven fabric.
[0184] Furthermore, the antithrombogenicity of Sample (3) of Example 3 was evaluated by a platelet adhesion test in the same manner as in Example 1. The results are shown in Figure 4C. From Figure 4C, almost no platelet adhesion was observed on the surface of Sample (3) of Example 3. From this, it is considered that Sample (3) of Example 3 has P(MEA-b-GMA)2, which has excellent antithrombogenicity, sufficiently immobilized on the fiber surface of the PET woven fabric.
[0185] In addition, a cylindrical polyethylene terephthalate (PET) woven fabric (diameter: 8 mm, length: 13 cm, thickness: 0.15 mm) with a stent sewn onto it was cut into a 3 cm cylindrical shape so that the sewn stent remained, and Sample (3-1) was prepared in the same manner as Sample (3), except that Sample (3-1) was used. The operability was evaluated using a force gauge in the same manner as in Example 1. The results are shown in Tables 1 and 2 below.
[0186] Example 4 1. Synthesis of MEA-GMA Block Copolymer [P(MEA-b-GMA)(4 / 1)] PolyGMA (PPO-GMA) having peroxide groups in the molecule was obtained in the same manner as in Example 2. Subsequently, 0.45 g of the obtained PPO-GMA (corresponding to 0.00315 mol of GMA) was used as a polymerization initiator to dissolve 1.8 g (0.0138 mol) of methoxyethyl acrylate (2-MTA, manufactured by Osaka Organic Chemical Industry Co., Ltd.) in 1,4-dioxane, and the resulting solution was polymerized at 80°C for 5 hours under a nitrogen atmosphere. The reaction product obtained after polymerization was reprecipitated with hexane and recovered to obtain a block copolymer (MEA:GMA = 4:1 (molar ratio)) (P(MEA-b-GMA)3) composed of methoxyethyl acrylate and glycidyl methacrylate as structural units.
[0187] 2. Preparation of Sample (4): Bonding of P(MEA-b-GMA)3 to PET Woven Fabric Sample (4) was prepared in the same manner as in Example 2, except that the P(MEA-b-GMA)3 obtained above was used instead of P(MEA-b-GMA)1 in Example 2. The glycidyl groups of P(MEA-b-GMA)3 were reacted with the hydroxyl or carboxyl groups on the surface of PET woven fabric 2 (plastic fabric substrate), thereby immobilizing P(MEA-b-GMA)3 (biocompatible layer) on PET woven fabric 2.
[0188] The surface of Sample (4) of Example 4 was observed with a scanning electron microscope (SEM). The results are shown in Figure 3. Figures 3G and 3H show SEM images at 200x and 1000x magnifications, respectively. Figure 3 shows that in Sample (4), P(MEA-b-GMA)3 can be selectively immobilized on the surface of a single fiber of the PET woven fabric without bridging between fibers. This is presumably because the P(MEA-b-GMA)3 terminal does not interact with the carboxyl or hydroxyl groups formed on the PET woven fabric.
[0189] Furthermore, sample (4) of Example 4 was evaluated for antithrombogenicity by a platelet adhesion test in the same manner as in Example 1. The results are shown in FIG. 4D. From FIG. 4D, almost no platelet adhesion was observed on the surface of sample (4) of Example 4. From this, it is considered that sample (4) of Example 4 has P(MEA-b-GMA)3, which has excellent antithrombogenicity, sufficiently immobilized on the fiber surface of the PET woven fabric.
[0190] In addition, sample (4-1) was prepared in the same manner as sample (4), except that a cylindrical polyethylene terephthalate (PET) woven fabric (diameter: 8 mm, length: 13 cm, thickness: 0.15 mm) with a stent sewn onto it was cut into a 3 cm cylindrical shape so that the sewn stent remained. The operability was evaluated using a force gauge in the same manner as in Example 1. The results are shown in Tables 1 and 2 below.
[0191] Comparative Example 1 1. Preparation of Plastic Fabric Substrate A cylindrical polyethylene terephthalate (PET) woven fabric (thickness: 0.15 mm) with a stent sewn thereon was cut into a 1 cm x 1 cm (1 cm 2 The PET woven fabric was cut into pieces of the same size as the PET woven fabric 1, immersed in ethanol for 1 minute, and then the ethanol was discarded. This procedure was repeated three times to perform washing (PET woven fabric 1).
[0192] 2. Preparation of Sample (5) The above-mentioned PET woven fabric 1 was immersed in a 10% by weight solution of 10% polymethoxyethyl acrylate (PMEA) in methanol (coating solution) at room temperature for 10 minutes (PET woven fabric 1'). Immediately after immersion, air bubbles were visible escaping from between the fibers. However, as the immersion continued, air bubbles ceased to appear, and after 10 minutes, no air bubbles were observed. Therefore, it was determined that the coating solution had completely permeated the PET woven fabric 1. The PET woven fabric 1' was removed from the coating solution and dried at 60°C for 10 minutes using a dryer to prepare Sample (5). Sample (5) has a structure in which a biocompatible layer containing PMEA is disposed on the PET woven fabric.
[0193] The surface of sample (5) of Comparative Example 1 was observed by SEM. The results are shown in Figure 5. Figures 5A and 5B show SEM images observed at 200x and 1000x magnifications, respectively. Figure 5 shows that in sample (5) of Comparative Example 1, a biocompatible layer was formed in which PMEA filled the spaces between the fibers.
[0194] In addition, sample (5-1) was prepared in the same manner as sample (5), except that a cylindrical polyethylene terephthalate (PET) woven fabric (diameter: 8 mm, length: 13 cm, thickness: 0.15 mm) with a stent sewn onto it was cut into a 3 cm cylindrical shape so that the sewn stent remained. The operability was evaluated using a force gauge in the same manner as in Example 1. The results are shown in Tables 1 and 2 below.
[0195] Comparative Example 2: From a cylindrical polyethylene terephthalate (PET) woven fabric (diameter: 8 mm, length: 13 cm, thickness: 0.15 mm) to which a stent was sewn, only the woven fabric was removed to a size of 1 cm x 1 cm (1 cm 2 The PET woven fabric 1 was cut into pieces of cloth measuring 1.5 mm in diameter, immersed in ethanol for 1 minute, and then discarded. This washing procedure was repeated three times (PET woven fabric 1). The PET woven fabric 1 thus obtained was designated as sample (6).
[0196] The antithrombogenicity of this PET woven fabric 1 (sample (6)) was evaluated by a platelet adhesion test in the same manner as in Example 1. The results are shown in Figure 6. From Figure 6, it can be seen that a large number of platelets adhered to the PET woven fabric 1 (sample (6) of Comparative Example 2) so as to fill the gaps between the fibers, indicating that the antithrombogenicity was poor.
[0197] In addition, sample (6-1) was prepared in the same manner as sample (6), except that a cylindrical polyethylene terephthalate (PET) woven fabric (diameter: 8 mm, length: 13 cm, thickness: 0.15 mm) with a stent sewn onto it was cut into a 3 cm cylindrical shape so that the sewn stent remained. The operability was evaluated using a force gauge in the same manner as in Example 1. The results are shown in Tables 1 and 2 below.
[0198]
[0199]
[0200] The results in Tables 1 and 2 show that Samples (1-1) to (4-1) of Examples 1 to 4 have loads significantly lower than Sample (5-1) of Comparative Example 1, and have loads comparable to Sample (6-1) of Comparative Example 2. Combined with the evaluation results of antithrombogenicity in the platelet adhesion test, it is expected that the medical device according to the present invention will be able to achieve both antithrombogenicity and operability.
[0201] This application is based on Japanese Patent Application No. 2023-56274, filed on March 30, 2023, the disclosure of which is hereby incorporated by reference in its entirety.
[0202] 10...plastic fabric substrate, 10a...substrate core portion, 10b...substrate surface layer, 11...biocompatible layer (antithrombogenic layer), 100...medical device.
Claims
1. A method for producing a medical device comprising a plastic cloth substrate and a biocompatible layer supported on at least a portion of the plastic cloth substrate, the biocompatible layer comprising a structural unit A derived from a monomer having a reactive group that reacts with a hydroxyl group in the molecule, and a polymerizable compound represented by the following formula (I): In the above formula (I), R 1 represents a hydrogen atom or a methyl group; X represents a group represented by the formula: -O-(R 2 O) m -R 3 or a tetrahydrofurfuryloxy group, in which R 2 each independently represents a linear or branched alkylene group having 1 to 4 carbon atoms; R 3 represents a linear or branched alkyl group having 1 to 4 carbon atoms, and m represents an integer of 1 to 5; subjecting the plastic fabric substrate to a plasma treatment to generate hydroxyl groups on the surface of the plastic fabric substrate; and reacting the hydroxyl groups with the reactive groups.
2. The method according to claim 1, wherein the copolymer is a random copolymer and has a carboxyl group at least at one end.
3. The method of claim 2, wherein the carboxyl group is derived from at least one compound selected from the group consisting of 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]tetrahydrate, and 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine)]hydrate.
4. The method of claim 1, wherein the copolymer is a block copolymer composed of structural units A and B.
5. The reactive group is a primary amino group (-NH 2 2. The method of claim 1 , wherein the aryl group is an aryl group or an epoxy group.
6. The method of claim 1, wherein the structural unit A is derived from at least one monomer selected from the group consisting of aminomethylacrylamide, aminomethylmethacrylamide, aminoethylacrylamide, aminoethylmethacrylamide, aminopropylacrylamide, aminopropylmethacrylamide (APMA), aminobutylacrylamide, aminobutylmethacrylamide, and salts thereof, glycidyl acrylate, glycidyl methacrylate (GMA), 3,4-epoxycyclohexylmethyl acrylate, 3,4-epoxycyclohexylmethyl methacrylate, β-methylglycidyl acrylate, and β-methylglycidyl methacrylate.
7. The method of claim 1, wherein the structural unit B is derived from at least one monomer selected from the group consisting of methoxymethyl acrylate, methoxyethyl acrylate (MEA), methoxypropyl acrylate, ethoxymethyl acrylate, ethoxyethyl acrylate, ethoxypropyl acrylate, ethoxybutyl acrylate, propoxymethyl acrylate, butoxyethyl acrylate, methoxybutyl acrylate, methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, propoxymethyl methacrylate, butoxyethyl methacrylate, and tetrahydrofurfuryl acrylate.
8. The method of claim 1, wherein the plastic is at least one selected from the group consisting of polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), and polybutylene terephthalate (PBT).
9. The method of claim 1, wherein the medical device is an artificial blood vessel, a stent graft, a covered stent or a catheter.
Citation Information
Patent Citations
Polyethylene glycol bipolymer with endothelial cell selectivity and preparation method and application method of composite coating
CN105713152A
Medical instrument having lubricating ability when wetted
JP1994285152A
Medical device
JP1994304243A
Method for hydrophilizing hydrophobic polymers
JP1998502857A
Antithrombogenic material and its manufacture process
JP2009153586A