Honeycomb structure, electric heating type carrier, and exhaust gas purification device

The honeycomb structure's tailored composition and resistivity control address the issue of uneven heating in EHC systems, ensuring uniform heat distribution and improved performance across varying voltages, thus enhancing the reliability and efficiency of electrically heated carriers in exhaust gas purification.

WO2024203087A1PCT designated stage expired Publication Date: 2024-10-03NGK INSULATORS LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008588
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-06
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional electrically heated catalyst (EHC) systems face challenges in achieving uniform heat generation distribution due to the NTC thermistor properties of silicon and silicon carbide, leading to uneven heating and increased risk of cracks, especially when used with varying vehicle voltages and low voltage power supplies.

Method used

A honeycomb structure with specific compositions of silicon and silicon carbide, optimized dopant concentrations, and porosity levels to relax NTC thermistor characteristics, ensuring uniform heat generation distribution by controlling the electrical resistivity across the structure.

Benefits of technology

The optimized honeycomb structure achieves significant improvement in heat generation uniformity, reducing the risk of cracks and enhancing the performance of electrically heated carriers in exhaust gas purification devices across a range of voltages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008588_03102024_PF_FP_ABST
    Figure JP2024008588_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a honeycomb structure having improved uniformity of heat generation distribution. This honeycomb structure comprises: a ceramic honeycomb structure part; and a pair of electrode layers that are provided on the outer surface of an outer peripheral wall, that extend in form of a band in a direction in which a cell extends, and that are provided so as to face each other across the central axis of the honeycomb structure part, the ceramic containing at least silicon and silicon carbide, and one or both of the following conditions (1) and (2) being met. (1) The silicon content of the ceramic is 21 to 30% by mass, the silicon contains P and B, and the value obtained by subtracting the concentration of B from the concentration of P in the silicon (P–B) is 20 mass ppm or more. (2) The silicon carbide content of the ceramic is 50% by mass or more, the silicon carbide contains Al and N, and the value obtained by subtracting the N concentration from the Al concentration in the silicon carbide (Al–N) is 130 mass ppm or more and 450 mass ppm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Honeycomb structure, electrically heated carrier and exhaust gas purification device

[0001] The present invention relates to a honeycomb structure, an electrically heated carrier including the honeycomb structure, and an exhaust gas purification device including the electrically heated carrier.

[0002] Conventionally, catalysts supported on honeycomb structures made of cordierite or silicon carbide have been used to treat harmful substances in exhaust gases emitted from automobile engines. When treating exhaust gases using a catalyst supported on a honeycomb structure, the catalyst must be heated to a predetermined temperature. However, a problem has traditionally arisen in that the catalyst temperature is low at engine start-up, preventing sufficient purification of the exhaust gas. To address this problem, a system called an electrically heated catalyst (EHC) has been developed. This system involves arranging electrodes on a honeycomb structure made of conductive ceramics, and heating the honeycomb structure itself by passing electricity through it, thereby heating the catalyst supported on the honeycomb structure to its activation temperature before or during engine start-up.

[0003] An EHC generally includes an outer peripheral wall, a conductive honeycomb structure portion disposed inside the outer peripheral wall and having partition walls that define a plurality of cells that form flow paths from a first end face to a second end face, and a pair of electrode layers disposed on the outer peripheral wall of the honeycomb structure portion. When an EHC is mounted on, for example, an automobile, the EHC shares a common power source with the electrical system of the automobile. Therefore, excessive current flowing through the EHC may damage the power supply circuit. Because various voltages are used for the power source of the EHC, it is important to adjust the resistance of the honeycomb structure for the EHC for each voltage to prevent excessive current flow.

[0004] Patent Document 1 describes a honeycomb structure in which the partition walls and peripheral walls contain silicon carbide particles as aggregate and silicon as a binder that bonds the silicon carbide particles, and the honeycomb structure has a volume electrical resistance of 1 to 40 Ωcm at 400°C. Patent Document 1 describes that by setting the average particle diameter of the silicon carbide particles to 3 to 40 μm, the volume electrical resistance of the honeycomb structure at 400°C can be set to 1 to 40 Ωcm. It also describes that because the honeycomb structure has a volume electrical resistance of 1 to 40 Ωcm at 400°C, even when a current is passed through it using a high-voltage power supply, excessive current does not flow, making it suitable for use as a heater.

[0005] However, a wide range of voltages is used for the power supply of an EHC, depending on, for example, the type of vehicle in which it is installed. In particular, when a low voltage of 60 V or less, for example 48 V, is used for the power supply of an EHC, the volume resistivity appropriate for suppressing the generation of excess current is around 0.1 Ω cm. As such, in recent EHCs that use a wide range of voltages, research and development of technology that effectively suppresses the generation of excess current even when used at low voltages is desired.

[0006] Therefore, Patent Documents 2 and 3 specify the range of the amount of dopant contained in the silicon constituting the EHC. In Patent Documents 2 and 3, the concentration of the dopant in the silicon in the ceramic constituting the partition walls and the outer wall of the honeycomb structure is set to 1×10 16 ~5 x 10 20 pieces / cm 3 It is stated that:

[0007] Another issue with EHCs is the uniformity of heat generation distribution. Because the honeycomb structure typically has a higher electrical resistivity than the electrode layer, current from the terminals connected to the electrode layer tends to be spread in the electrode layer before flowing to the honeycomb structure. This causes a large amount of current to flow near the ends of the electrode layer, where the distance through the honeycomb structure is shorter. This results in uneven heat generation distribution in the honeycomb structure, leading to the problem of uneven catalyst heating. Poor heat generation distribution tends to result in excessive heat generation in parts of the EHC, increasing the likelihood of cracks.

[0008] Therefore, Patent Document 4 proposes controlling the distribution of electrical resistivity in end regions near a pair of electrodes of a honeycomb structure and in a central region excluding the end regions. Specifically, it proposes improving the uniformity of heat distribution in the honeycomb structure by making the average electrical resistivity of the material constituting the end regions lower than the average electrical resistivity of the material constituting the central region.

[0009] Japanese Patent No. 5735428 Japanese Patent Application Laid-Open No. 2020-204300 Japanese Patent Application Laid-Open No. 2022-142543 Japanese Patent Application Laid-Open No. 2019-173662

[0010] As proposed in Patent Documents 2 and 3, controlling the concentration of dopants in silicon in the ceramics that constitute the partition walls and outer wall of a honeycomb structure is useful for adjusting the volume resistivity of the honeycomb structure. Furthermore, as proposed in Patent Document 4, controlling the distribution of electrical resistivity within the honeycomb structure is also useful for improving the uniformity of heat generation distribution. However, with honeycomb structures containing dopants, there remains room for improving the uniformity of heat generation distribution using methods different from those used so far.

[0011] The present invention has been made in view of the above circumstances, and an object of one embodiment is to provide a honeycomb structure in which the uniformity of heat distribution is improved by a method different from that of the conventional method.

[0012] The present inventors conducted extensive research to solve the above-mentioned problems and found that the non-uniformity of heat generation distribution in a honeycomb structure is due to the conventionally known cell structure of the honeycomb structure, as well as the NTC thermistor characteristics of the silicon carbide and silicon materials that make up the honeycomb structure. In other words, the NTC thermistor characteristics of silicon and silicon carbide further reduce the electrical resistance at the ends of the electrode layers of the honeycomb structure, which are prone to heat generation, making it easier for electricity to flow (i.e., easier to generate heat). It was found that repeated occurrence of this leads to a large deviation in the heat generation distribution in a cross section perpendicular to the extension direction of the cells of the honeycomb structure, increasing the probability of cracks occurring.

[0013] Therefore, the present inventors have considered that alleviating the NTC thermistor characteristics is important for improving the uniformity of heat generation distribution in a honeycomb structure, and have conducted extensive research. As a result, the present inventors have found that the NTC thermistor characteristics can be alleviated and the uniformity of heat generation distribution in a honeycomb structure can be significantly improved by appropriately controlling the contents of silicon carbide and silicon and the concentration of a predetermined dopant. The present invention was completed based on this finding, and is exemplified below. [Aspect 1] A honeycomb structure comprising: a ceramic honeycomb structure part having an outer peripheral wall and partition walls disposed inside the outer peripheral wall to separate a plurality of cells that form a fluid flow path from a first end face to a second end face; and a pair of electrode layers disposed on the outer surface of the outer peripheral wall, extending in a strip-like shape in the extension direction of the cells, and disposed opposite to each other across a central axis of the honeycomb structure part; wherein the ceramic contains at least silicon and silicon carbide, and satisfies one or both of the following conditions (1) and (2): (1) The ceramic has a silicon content of 21 to 30 mass%, the silicon contains P and B, and the value obtained by subtracting the B concentration from the P concentration in the silicon (P-B amount) is 20 mass ppm or more. (2) The ceramic has a silicon carbide content of 50 mass% or more, the silicon carbide contains Al and N, and the value obtained by subtracting the N concentration from the Al concentration in the silicon carbide (Al-N amount) is 130 mass ppm or more and 450 mass ppm or less. [Aspect 2] The honeycomb structure according to aspect 1, which satisfies both of the conditions (1) and (2). [Aspect 3] The honeycomb structure according to aspect 1 or 2, wherein the ceramic satisfies one or both of the following conditions (3) and (4). (3) The ceramic has a silicon content of 21 to 30 mass%, the silicon contains P and B, and the value obtained by subtracting the B concentration from the P concentration in the silicon (P-B amount) is 20 mass ppm or more. (4) The ceramic has a silicon carbide content of 50 mass% or more, the silicon carbide contains Al and N, and the value obtained by subtracting the N concentration from the Al concentration in the silicon carbide (Al-N amount) is 300 mass ppm or more and 450 mass ppm or less. [Aspect 4] A honeycomb structure according to aspect 3, which satisfies both of the conditions (3) and (4).[Aspect 5] The honeycomb structure according to any one of Aspects 1 to 4, wherein the total content of silicon and silicon carbide in the ceramic is 80 to 95 mass %. [Aspect 6] The honeycomb structure according to any one of Aspects 1 to 5, wherein the ceramic further contains 5 to 20 mass % of silicon oxide. [Aspect 7] The honeycomb structure according to any one of Aspects 1 to 6, wherein the porosity of the partition walls of the honeycomb structure part is 30% or more. [Aspect 8] The volume resistivity (ρ) of the honeycomb structure part at 50°C. v50 ) versus volume resistivity at 500 ° C. (ρ v500 ) ratio (ρ v500 / ρ v50 The honeycomb structure according to any one of Aspects 1 to 7, characterized in that the value of the surface roughness (Tc) of the conductive layer is 0.30 to 0.80. [Aspect 9] An electrically heated carrier comprising: the honeycomb structure according to any one of Aspects 1 to 8; and metal terminals joined to outer surfaces of the pair of electrode layers, respectively. [Aspect 10] An exhaust gas purification device comprising: the electrically heated carrier according to Aspect 9; and a metal tube accommodating the electrically heated carrier.

[0014] According to one embodiment of the present invention, a honeycomb structure with improved uniformity of heat generation distribution can be provided. Further improvement in uniformity of heat generation distribution can be expected by combining this with other conventionally known techniques. An electrically heated carrier can be produced by joining a metal terminal to this honeycomb structure. The electrically heated carrier can be suitably used, for example, as a catalyst carrier for an exhaust gas purification device.

[0015] 1 is a schematic diagram of an electrically heated carrier according to an embodiment of the present invention when observed from a first end face. 2 is a schematic perspective view of an electrically heated carrier according to an embodiment of the present invention. 3 is a schematic cross-sectional view showing an exhaust gas purification device according to an embodiment of the present invention.

[0016] Next, embodiments of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiments, and that appropriate design changes and improvements may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.

[0017] (1. Electrically Heated Carrier) Fig. 1 is a schematic diagram of an electrically heated carrier 100 according to one embodiment of the present invention when viewed from a first end surface 116. Fig. 2 is a schematic perspective view of the electrically heated carrier 100 according to one embodiment of the present invention.

[0018] The electrically heated carrier 100 includes a honeycomb structure 110 and a metal terminal 130. By supporting a catalyst on the electrically heated carrier 100, the electrically heated carrier 100 can be used as a catalyst body. Examples of the catalyst include precious metal catalysts and other catalysts. Precious metal catalysts include three-way catalysts and oxidation catalysts in which a precious metal such as platinum (Pt), palladium (Pd), or rhodium (Rh) is supported on the surface of alumina pores and a promoter such as ceria or zirconia is included, or alkaline earth metals and platinum are used to reduce nitrogen oxides (NO x ) as a storage component of NO x Examples of catalysts that do not use precious metals include NOx storage reduction catalysts (LNT catalysts) containing copper-substituted or iron-substituted zeolites. x Examples of the catalyst include a selective catalytic reduction catalyst (SCR catalyst). Two or more catalysts selected from these catalysts may be used. There are no particular limitations on the method for supporting the catalyst, and any known method for supporting a catalyst on a honeycomb structure may be used.

[0019] (1-1. Honeycomb structure) In one embodiment, the honeycomb structure 110 comprises: a ceramic honeycomb structure part having an outer peripheral wall 114 and partition walls 113 disposed inside the outer peripheral wall 114 and dividing a plurality of cells 115 that form flow paths from a first end face 116 to a second end face 118; a first electrode layer 112a disposed on the outer surface of the outer peripheral wall 114 and extending in a strip-like shape in the extension direction of the cells 115; and a second electrode layer 112b disposed on the outer surface of the outer peripheral wall 114 and extending in a strip-like shape in the extension direction of the cells 115, the second electrode layer 112b being disposed opposite to the first electrode layer 112a across the central axis O of the honeycomb structure part.

[0020] The outer shape of the honeycomb structure 110 is not particularly limited, and may be, for example, a columnar body having a round end face such as a circular, oval, elliptical, racetrack, or oval shape, a columnar body having a polygonal end face such as a triangular or rectangular shape, or a columnar body having an end face with other irregular shapes. The illustrated honeycomb structure 110 has a circular end face shape and is cylindrical as a whole.

[0021] There is no particular limitation on the height of the honeycomb structure 110 (the length from one end face to the other end face), and it may be set appropriately depending on the application and required performance. There is also no particular limitation on the relationship between the height of the honeycomb structure 110 and the maximum diameter of each end face (the maximum length of the diameters passing through the center of gravity of each end face of the honeycomb structure). Therefore, the height of the honeycomb structure 110 may be longer than the maximum diameter of each end face, or the height of the honeycomb structure 110 may be shorter than the maximum diameter of each end face.

[0022] The size of the honeycomb structure 110 is set to 2000 to 20000 mm2 in order to improve heat resistance (to suppress cracks in the circumferential direction of the outer peripheral wall). 2 It is preferable that the thickness is 5000 to 15000 mm 2 It is more preferable that:

[0023] <Honeycomb Structure Portion> The ceramic honeycomb structure portion has a higher volume resistivity than the electrode layers 112a and 112b, but is conductive. The volume resistivity of the honeycomb structure portion is not particularly limited as long as it can generate heat by Joule heating when current is applied, and can be set appropriately depending on the applied voltage. For example, when measured at 25°C, the volume resistivity can be 0.001 to 500 Ω·cm. For high voltages greater than 60 V, the volume resistivity can be 2 to 100 Ω·cm, typically 5 to 100 Ω·cm. For low voltages of 60 V or less, such as 48 V, the volume resistivity can be 0.001 to 2 Ω·cm, typically 0.001 to 1 Ω·cm, and more typically 0.01 to 1 Ω·cm.

[0024] In one embodiment, the volume resistivity (ρ) of the honeycomb structure at 50°C v50 ) versus volume resistivity at 500 ° C. (ρ v500) ratio (ρ v500 / ρ v50 ) is 0.30 or more. v500 / ρ v50 When ρ is 0.30 or more, it means that the NTC thermistor characteristics are relaxed, and the uniformity of the heat generation distribution is significantly improved. v500 / ρ v50 is preferably 0.35 or more, more preferably 0.40 or more. In addition, since a silicon-silicon carbide composite material or a ceramic material containing silicon carbide as a main component is used in the honeycomb structure, ρ v500 / ρ v50 The upper limit of is preferably 0.80 or less, more preferably 0.75 or less, and even more preferably 0.70 or less. v500 / ρ v50 is, for example, preferably 0.30 to 0.80, more preferably 0.35 to 0.75, and even more preferably 0.40 to 0.70.

[0025] In this specification, the volume resistivity of a honeycomb structure part is measured by the following procedure. A total of five partition wall samples, each measuring 5 mm × 5 mm × 50 mm (in the cell extension direction), are taken from the honeycomb structure part, and the volume resistivity of each is measured at 25°C by the four-terminal method unless otherwise specified, and the average value of the five samples is taken as the volume resistivity of the honeycomb structure part. The partition wall samples are taken from the vicinity of the center in the height direction and the radial direction of the honeycomb structure part.

[0026] In one embodiment, the ceramic constituting the honeycomb structure portion having the outer peripheral wall 114 and the partition walls 113 contains at least (metallic) silicon and silicon carbide, and preferably the total content of silicon and silicon carbide in the ceramic is 80 to 95 mass%. Typically, the ceramic contains a silicon carbide-silicon composite. From the viewpoint of achieving both heat resistance and electrical conductivity, the ceramic preferably contains a silicon carbide-silicon composite as its main component. When the ceramic contains a silicon carbide-silicon composite as its main component, this means that the silicon carbide-silicon composite (total mass) in the ceramic accounts for 70 mass% or more of the total, preferably 80 to 95 mass%. From the viewpoint of alleviating the NTC thermistor characteristics, it is advantageous to adjust the silicon and silicon carbide contents in the ceramic constituting the honeycomb structure portion.

[0027] Here, the silicon carbide-silicon composite material contains silicon carbide particles as an aggregate and (metallic) silicon as a binder that binds the silicon carbide particles. The ceramic may contain, in addition to silicon carbide particles, one or two aggregates selected from silicon nitride particles and aluminum nitride particles. It may also contain one or more other aggregates. Examples of other aggregates include oxide ceramics such as alumina, mullite, zirconia, and cordierite.

[0028] However, if the main component of the aggregate is silicon carbide, it is preferable because the thermal conductivity is higher and the difference in thermal expansion coefficient with silicon is smaller. When the main component of the aggregate is silicon carbide, it means that silicon carbide (total mass) accounts for 80 mass% or more of the aggregate, and more preferably 90 mass% or more of the aggregate.

[0029] The silicon and silicon carbide in the ceramics constituting the honeycomb structure portion can contain one or more dopants. The dopants in the silicon and silicon carbide can be, for example, one or more selected from Group 13 and Group 15 elements of the periodic table. For example, Group 13 elements include boron (B), aluminum (Al), gallium (Ga), and indium (In), while Group 15 elements include nitrogen (N), phosphorus (P), arsenic (As), antimony (Sb), and bismuth (Bi). Among these, from the viewpoint of alleviating the NTC thermistor characteristics, it is preferable to control at least one of the value obtained by subtracting the B concentration from the P concentration in silicon (P-B amount) and the value obtained by subtracting the N concentration from the Al concentration in silicon carbide (Al-N amount), and more preferably, to control both.

[0030] Therefore, in a honeycomb structure according to one embodiment of the present invention, the silicon content, the silicon carbide content, the value obtained by subtracting the B concentration from the P concentration in silicon (P-B content), and the value obtained by subtracting the N concentration from the Al concentration in silicon carbide (Al-N content) in the ceramics constituting the honeycomb structure part preferably satisfy at least one of the following conditions (1) and (2), and more preferably satisfy both conditions: (1) The silicon content in the ceramics is 21 to 30 mass%, the silicon contains P and B, and the P-B content in the silicon is 20 ppm by mass or more; (2) The silicon carbide content in the ceramics is 50 mass% or more, the silicon carbide contains Al and N, and the Al-N content in the silicon carbide is 130 ppm by mass or more and 450 ppm by mass or less.

[0031] It is more preferable that the ceramics satisfy at least one of the following conditions (3) and (4), and it is even more preferable that the ceramics satisfy both conditions: (3) The silicon content in the ceramics is 21 to 30 mass%, the silicon contains P and B, and the P-B content in the silicon is 20 mass ppm or more; (4) The silicon carbide content in the ceramics is 50 mass% or more, the silicon carbide contains Al and N, and the Al-N content in the silicon carbide is 300 mass ppm or more and 450 mass ppm or less.

[0032] The amount of P-B in the silicon contained in the ceramics may be 20 ppm by mass or more, and preferably 25 ppm by mass or more. There is no particular upper limit for the amount of P-B in the silicon contained in the ceramics, but considering the concentrations of P and B generally added as dopants in silicon, it is usually 100 ppm by mass or less, and typically 90 ppm by mass or less. Therefore, the amount of P-B in the silicon contained in the ceramics is preferably, for example, 20 to 100 ppm by mass, more preferably 25 to 90 ppm by mass, and can be, for example, 20 to 50 ppm by mass.

[0033] From the viewpoint of making the volume resistivity of silicon uniform, the upper limit of the B concentration in the silicon contained in the ceramic is preferably 60 mass ppm or less, more preferably 50 mass ppm or less. Furthermore, even in generally high-purity silicon, a small amount of B is added as a dopant, and the B concentration is 10 mass ppm or more. Therefore, the B concentration in the silicon contained in the ceramic is, for example, preferably 10 to 60 mass ppm, more preferably 10 to 50 mass ppm, and can be, for example, 10 to 20 mass ppm.

[0034] As the N dopant concentration in silicon carbide increases, the electrical resistance of the honeycomb structure tends to decrease. From the viewpoint of keeping the electrical resistance of the honeycomb structure within a predetermined range, the N concentration in silicon carbide is, for example, preferably 50 to 500 ppm by mass, more preferably 50 to 450 ppm by mass, and can be, for example, 50 to 200 ppm by mass, or can also be 60 to 120 ppm by mass.

[0035] From the viewpoint of alleviating the NTC thermistor characteristics, it is preferable to also control the silicon oxide content in the ceramics constituting the honeycomb structure portion. The silicon oxide content in the ceramics is preferably 5 to 20 mass %, for example, 10 to 15 mass %.

[0036] The contents of Si (silicon), SiC (silicon carbide), and SiO2 (silicon oxide) in the ceramics constituting the honeycomb structure can be measured by the following method. The following method describes a calculation method when (doped) silicon and silicon carbide are used as the ceramic raw materials. When silicon and silicon carbide are used as the ceramic raw materials, the ceramics constituting the honeycomb structure are composed of silicon (Si), silicon carbide (SiC), and silicon oxide (SiO2). The contents of Si (silicon), SiC (silicon carbide), and SiO2 (silicon oxide) in the ceramics can be measured by measuring the silicon element amount and oxygen element amount using an X-ray fluorescence method, and measuring the carbon element amount using a resistance heating infrared absorption method. Measurement samples are taken from near the center of the honeycomb structure in the height direction and radial direction. Each sample has a mass of 10 g. The average values ​​of the contents of each component in the five samples are taken as the contents of Si (silicon), SiC (silicon carbide), and SiO2 (silicon oxide) in the ceramic.

[0037] Regarding the amount of SiC (silicon carbide), all carbon elements are assumed to be SiC, and the amount of SiC in the ceramic is calculated by molecular weight calculation. Regarding the amount of SiO2 (silicon oxide), all oxygen elements are assumed to be SiO2, and the amount of SiO2 in the ceramic is calculated by molecular weight calculation. The amount of Si (silicon) can be calculated by subtracting the total amount of Si, which is the sum of the amount of Si in SiC and the amount of Si in SiO2, from the total amount of silicon element from the amounts of SiC and SiO2 calculated above. When a ceramic raw material other than silicon carbide is used, the composition of the ceramics constituting the honeycomb structure portion based on the ceramic raw material is confirmed, and then the amount of elements can be measured by X-ray fluorescence or resistance heating infrared absorption spectroscopy, and the amount can be calculated in the same way.

[0038] Regarding the P concentration and B concentration in silicon in the ceramics constituting the honeycomb structure part, a total of five partition wall samples, each weighing 10 g, are taken from near the center in the height direction and the center in the radial direction of the honeycomb structure part, and the P concentration and B concentration in silicon of each of the samples are measured by the following procedure, and the average value is calculated and used as the measured value.

[0039] The method for measuring the P and B concentrations in silicon (Si) in a partition wall sample is as follows. According to the silicon separation ICP atomic emission spectroscopy specified in JIS G1322-3:2010 "Metallic Silicon Analysis Method," the partition wall sample is decomposed with nitric acid and hydrofluoric acid, perchloric acid is added, and the sample is heated to generate white fumes of perchloric acid. The silicon is volatilized and separated as silicon tetrafluoride, and the salts are then dissolved in water. Next, the P and B contained in the solution are measured by ICP atomic emission spectroscopy, and the concentrations in the silicon are calculated.

[0040] The Al concentration and N concentration in silicon carbide in the ceramics constituting the honeycomb structure can be measured by the following method. First, a total of five partition wall samples are taken from the honeycomb structure near the center in the height direction and the diameter direction of the honeycomb structure. The size of one sample is 1 cm. 3 The size of the sample is 1 cm x 1 cm x 1 cm cube. The sample is observed with a scanning electron microscope (SEM) (magnification 1000x), and dark contrast areas are visually identified as silicon carbide portions. The silicon carbide portions are then analyzed by secondary ion mass spectrometry (SIMS) to determine the Al concentration and N concentration in the silicon carbide. The average values ​​of the Al concentration and N concentration in the five samples are taken as the Al concentration and N concentration in the silicon carbide of the ceramic.

[0041] The partition walls 113 of the honeycomb structure portion may be dense, such as in the form of Si-impregnated SiC, but are preferably porous. If the porosity of the partition walls 113 is 30% or more, deformation during firing is more easily suppressed. Furthermore, if the porosity of the partition walls 113 is 60% or less, the strength of the honeycomb structure portion is sufficiently maintained. Therefore, the porosity of the partition walls 113 is preferably, for example, 30% or more, more preferably 35 to 60% in order to keep the thermistor characteristics within a predetermined range, and even more preferably 37 to 45%. The porosity is a value measured using a mercury porosimeter. Note that dense refers to a porosity of 5% or less.

[0042] The thickness of the partition walls 113 that define the cells 115 is preferably 0.1 to 0.3 mm, and more preferably 0.1 to 0.2 mm. When the thickness of the partition walls 113 is 0.1 mm or more, it is possible to prevent a decrease in the strength of the honeycomb structure portion. When the thickness of the partition walls 113 is 0.3 mm or less, it is possible to prevent an increase in pressure loss when exhaust gas flows through the honeycomb structure portion when the honeycomb structure portion is used as a catalyst carrier and a catalyst is carried thereon. In the present invention, the thickness of the partition walls 113 is defined as the length of a portion of a line segment that connects the centers of gravity of adjacent cells 115 and that passes through the partition walls 113 in a cross section perpendicular to the extension direction of the cells 115.

[0043] Providing the honeycomb structure with the peripheral wall 114 is useful from the viewpoint of ensuring the structural strength of the honeycomb structure and suppressing leakage of the fluid flowing through the cells 115 from the peripheral wall 114. In this regard, the thickness of the peripheral wall 114 is preferably 0.1 mm or more, more preferably 0.15 mm or more, and even more preferably 0.2 mm or more. However, if the peripheral wall 114 is made too thick, it will have too high strength, which will disrupt the strength balance with the partition walls 113 and reduce thermal shock resistance. Therefore, the thickness of the peripheral wall 114 is preferably 1.0 mm or less, more preferably 0.7 mm or less, and even more preferably 0.5 mm or less. Therefore, the thickness of the peripheral wall 114 is preferably, for example, 0.1 to 1.0 mm, more preferably 0.15 to 0.7 mm, and even more preferably 0.2 to 0.5 mm. Here, the thickness of the outer peripheral wall 114 is defined as the thickness in the direction normal to the tangent to the outer surface of the outer peripheral wall 114 at the measurement point when the portion of the outer peripheral wall 114 where the thickness is to be measured is observed in a cross section perpendicular to the extension direction of the cell 115.

[0044] The honeycomb structure has a cell density of 40 to 150 cells / cm in a cross section perpendicular to the extension direction of the cells 115. 2 Preferably, the density is 70 to 100 cells / cm 2 By setting the cell density in this range, it is possible to increase the purification performance of the catalyst while reducing the pressure loss when exhaust gas flows through the honeycomb structure.2 If the cell density is 150 cells / cm or more, a sufficient catalyst carrying area is ensured. 2 When the honeycomb structure 110 is used as a catalyst carrier and a catalyst is carried thereon, the pressure loss during the flow of exhaust gas is prevented from becoming too large if the honeycomb structure 110 is used as a catalyst carrier and the cell density is a value obtained by dividing the number of cells by the area of ​​one end face of the honeycomb structure part on the inner peripheral side of the outer peripheral wall 114.

[0045] Although there are no limitations on the shape of the cells in a cross section perpendicular to the extension direction of the cells 115, a square, a hexagon, an octagon, or a combination thereof is preferred. Among these, a square and a hexagon are more preferred. By using such a cell shape, the pressure loss when exhaust gas flows through the honeycomb structure 110 is reduced, and the purification performance of the catalyst is improved. From the viewpoint of easily achieving both structural strength and heating uniformity, a hexagon is particularly preferred.

[0046] The cells 115 may penetrate from the first end face 116 to the second end face 118. In this case, the cells 115 may be open at both the first end face 116 and the second end face 118. Alternatively, first cells having plugged first end faces 116 and openings at the second end faces 118 and second cells having openings at the first end faces 116 and plugged second end faces 118 may be alternately arranged adjacent to each other with the partition wall 113 interposed therebetween.

[0047] <Electrode Layer> A first electrode layer 112a and a second electrode layer 112b facing the first electrode layer 112a across the central axis O of the honeycomb structure section can be provided on the outer surface of the outer peripheral wall 114. By providing the electrode layers 112a, 112b having a lower volume resistivity than the outer peripheral wall 114, current is more likely to spread in the circumferential direction of the honeycomb structure 110 and in the extension direction of the cells 115, thereby improving the uniform heat generation of the honeycomb structure 110. Referring to FIG. 1 , in a cross section perpendicular to the extension direction of the cells 115, the angle θ (0°≦θ≦180°) formed by two line segments extending from the circumferential centers of the pair of electrode layers 112a, 112b to the central axis O (center of gravity) of the honeycomb structure 110 is preferably 150°≦θ≦180°, more preferably 160°≦θ≦180°, even more preferably 170°≦θ≦180°, and most preferably 180°.

[0048] Although there are no particular restrictions on the formation regions of the pair of electrode layers 112a, 112b, from the viewpoint of improving the uniform heat generation of the honeycomb structure 110, it is preferable that the pair of electrode layers 112a, 112b are each provided in a band-like shape extending on the outer surface of the outer peripheral wall 114 in the circumferential direction of the honeycomb structure 110 and in the extension direction of the cells 115. Specifically, in a cross section perpendicular to the extension direction of the cells 115, the central angle α formed by two line segments connecting both circumferential ends of each electrode layer 112a, 112b to the central axis O (center of gravity) is preferably 30° or more, more preferably 40° or more, and even more preferably 60° or more, from the viewpoint of spreading the current in the circumferential direction and improving the uniform heat generation (see FIG. 1 ). However, if the central angle α is too large, less current passes through the interior of the honeycomb structure 110, and more current passes near the outer peripheral wall 114. Therefore, from the viewpoint of uniform heat generation of the honeycomb structure 110, the central angle α is preferably 140° or less, more preferably 130° or less, and even more preferably 120° or less. Furthermore, it is desirable that each of the electrode layers 112a, 112b extends over 80% or more of the length between both end faces of the honeycomb structure 110, preferably over 90% or more, and more preferably over the entire length. The electrode layers 112a, 112b may be composed of a single layer, or may have a laminated structure in which multiple layers are stacked.

[0049] The thickness of the electrode layers 112a, 112b is preferably 0.01 to 5 mm, and more preferably 0.01 to 3 mm. Setting the thickness within this range can improve uniform heat generation. When the thickness of the electrode layers 112a, 112b is 0.01 mm or more, the electrical resistance is appropriately controlled, allowing for more uniform heat generation. When the thickness of the electrode layers 112a, 112b is 5 mm or less, the risk of breakage during canning is reduced. The thickness of the electrode layers 112a, 112b is defined as the thickness in the direction normal to the tangent to the outer surface of the electrode layers 112a, 112b at the measurement location when the location of the electrode layers 112a, 112b where the thickness is to be measured is observed in a cross section perpendicular to the extension direction of the cell 115.

[0050] By making the volume resistivity of the electrode layers 112a, 112b lower than the volume resistivity of the partition walls 113 and the outer peripheral wall 114, electricity flows preferentially through the electrode layers 112a, 112b, and when energized, electricity spreads more easily in the circumferential direction of the honeycomb structure 110 and in the extension direction of the cells 115. The volume resistivity of the electrode layers 112a, 112b is preferably 1 / 10 or less of the volume resistivity of the partition walls 113 and the outer peripheral wall 114, more preferably 1 / 20 or less, and even more preferably 1 / 30 or less. However, if the difference in volume resistivity between the two becomes too large, current will concentrate between the ends of the opposing electrode layers 112a, 112b, causing uneven heat generation in the honeycomb structure 110. Therefore, the volume resistivity of the electrode layers 112a, 112b is preferably 1 / 200 or more, more preferably 1 / 150 or more, and even more preferably 1 / 100 or more of the volume resistivity of the partition walls 113 and the outer peripheral wall 114. Therefore, the volume resistivity of the electrode layers 112a, 112b is, for example, preferably 1 / 200 to 1 / 10 of the volume resistivity of the partition walls 113 and the outer peripheral wall 114, more preferably 1 / 150 to 1 / 20, and even more preferably 1 / 100 to 1 / 30. The volume resistivities of the electrode layers, partition walls, and outer peripheral wall herein are values ​​measured at 25°C by a four-terminal method.

[0051] The material of the electrode layers 112a and 112b is not limited to, but may be a composite (cermet) of metal and ceramic (especially conductive ceramic). Examples of metals include, for example, Cr, Fe, Co, Ni, Si, or Ti, or alloys containing at least one metal selected from these metals. Examples of ceramics include, but are not limited to, silicon carbide (SiC), as well as metal compounds such as metal silicides, such as tantalum silicide (TaSi) and chromium silicide (CrSi). Specific examples of composites (cermets) of metal and ceramic include composites of silicon and silicon carbide, composites of silicon and metal silicides, such as tantalum silicide or chromium silicide, and composites in which one or more of the above metals are added with one or more insulating ceramics, such as alumina, mullite, zirconia, cordierite, silicon nitride, and aluminum nitride, in order to reduce thermal expansion. As the material for the electrode layers 112a, 112b, among the various metals and ceramics described above, a composite material of a metal silicide such as tantalum silicide or chromium silicide, silicon, and silicon carbide is preferred because it can be fired simultaneously with the partition wall and the outer peripheral wall, thereby contributing to simplification of the manufacturing process.

[0052] (1-2. Metal Terminal) The metal terminal 130 can be directly or indirectly bonded to the outer surfaces of each of the pair of electrode layers 112a, 112b. When a voltage is applied to the honeycomb structure 110 via the metal terminal 130, electricity flows and the honeycomb structure 110 can generate heat by Joule heat. Therefore, the honeycomb structure 110 can also be suitably used as a heater. This makes it possible to improve the uniform heat generation of the honeycomb structure 110. The applied voltage is preferably 12 to 900 V, more preferably 48 to 600 V, but the applied voltage can be changed as appropriate.

[0053] The metal terminal 130 and the electrode layers 112a, 112b may be directly bonded to each other, or may be bonded to each other via one or more base layers 120 in order to reduce the difference in thermal expansion between the electrode layers 112a, 112b and the metal terminal 130 and thereby improve the bonding reliability of the metal terminal 130. Therefore, in a preferred embodiment, the honeycomb structure 110 has a first electrode layer 112a and a second electrode layer 112b disposed on the outer peripheral wall 114 so as to face each other across the central axis O (center of gravity) of the honeycomb structure 110, and one or more metal terminals 130 are bonded to each of the electrode layers 112a, 112b via the base layer 120.

[0054] From the viewpoint of improving bonding reliability, it is preferable that the thermal expansion coefficient gradually decreases in the order of the metal terminal 130 → (underlying layer 120) → electrode layers 112a and 112b → outer peripheral wall 114. Note that the "thermal expansion coefficient" here refers to the linear expansion coefficient measured in accordance with JIS R1618:2002 when the temperature is changed from 25°C to 800°C.

[0055] The material of the metal terminal 130 is not particularly limited as long as it is a metal, and simple metals and alloys can be used, but from the viewpoints of corrosion resistance, volume resistivity, and linear expansion coefficient, an alloy containing at least one selected from the group consisting of Cr, Fe, Co, Ni, and Ti is preferable, and stainless steel and an Fe-Ni alloy are more preferable. The number, shape, and size of the metal terminals 130 are not particularly limited, and can be designed appropriately depending on the size, electrical conductivity, etc. of the honeycomb structure 110.

[0056] The material of the base layer 120 is not limited, but may be a composite material (cermet) of metal and ceramic (particularly conductive ceramic). The thermal expansion coefficient of the base layer 120 can be controlled by adjusting the compounding ratio of the metal and ceramic, for example.

[0057] The underlayer 120 preferably contains, but is not limited to, one or more metals selected from Ni-based alloys, Fe-based alloys, Ti-based alloys, Co-based alloys, silicon, and Cr.

[0058] The underlayer 120 preferably contains one or more ceramics selected from, but not limited to, oxide ceramics such as alumina, mullite, zirconia, glass, and cordierite, and non-oxide ceramics such as silicon carbide, silicon nitride, and aluminum nitride.

[0059] The thickness of the base layer 120 is not particularly limited, but is preferably 0.1 to 1.5 mm, and more preferably 0.3 to 0.5 mm, from the viewpoint of crack suppression. The thickness of the base layer 120 is defined as the thickness in the direction normal to the tangent to the outer surface of the base layer 120 at the measurement point when the base layer 120 whose thickness is to be measured is observed in a cross section perpendicular to the extension direction of the cells.

[0060] The method for joining the metal terminal 130 to the electrode layers 112a, 112b or the base layer 120 is not particularly limited, but examples thereof include thermal spraying, welding, and brazing.

[0061] (2. Exhaust Gas Purification Apparatus) An electrically heated carrier according to one embodiment of the present invention can be used in an exhaust gas purification apparatus. Referring to FIG. 3, an exhaust gas purification apparatus 200 has an electrically heated carrier 100 and a metal tube 220 that houses the electrically heated carrier 100. An electric wire 240 for supplying power can be connected to a metal terminal 130 of the electrically heated carrier 100. Metals that constitute the metal tube 220 include, but are not limited to, various stainless steels such as chromium-based stainless steel. The use of these metals results in an exhaust gas purification apparatus with high heat resistance and corrosion resistance.

[0062] In the exhaust gas purification device 200, the electrically heated carrier 100 can be installed midway through the flow path of a fluid such as automobile exhaust gas. The electrically heated carrier 100 can be fixed inside the metal tube 220, for example, by push-in canning, in which the electrically heated carrier 100 is pushed into the metal tube 220 and fitted into the metal tube 220 in a positional relationship in which the extension direction of the cells and the extension direction of the metal tube 220 coincide. It is preferable to dispose a holding material (mat) 260 between the metal tube 220 and the electrically heated carrier 100. The material constituting the holding material (mat) 260 is not limited, but examples include ceramics such as alumina fiber, mullite fiber, and ceramic fiber mainly composed of alumina-silica.

[0063] (3. Manufacturing Method) Next, a method for manufacturing a honeycomb structure according to one embodiment of the present invention will be described. The honeycomb structure can be manufactured by a manufacturing method including step 1 of preparing a clay, step 2 of molding the clay to obtain a honeycomb formed body, step 3 of applying a pair of electrode layer forming pastes to the outer surface of the peripheral wall so that the pastes extend in strips in the extension direction of the cells across the central axis of the honeycomb formed body, thereby manufacturing a honeycomb formed body with the electrode layer forming pastes, and step 4 of firing the honeycomb formed body to manufacture a honeycomb fired body.

[0064] (Step 1) In step 1, a molding raw material containing silicon carbide powder and (metallic) silicon powder is kneaded to prepare a clay. One or both of the silicon carbide powder and silicon powder can be appropriately doped with a dopant such as B, Al, N, or P. The dopant concentrations in the silicon carbide powder and silicon powder can be adjusted, for example, by adding a trace amount of dopant element during the production of the molding raw material, or by mixing molding raw materials having different dopant amounts in any ratio. Also, for doping silicon with P and B, an aqueous solution containing a predetermined amount of dopant source (such as a water-soluble inorganic salt or a water-soluble organic compound) can be kneaded with the molding raw material to incorporate the dopant source into the clay, and then doping during firing can be performed.

[0065] The mass of the metal silicon powder in the forming raw material is preferably 20 to 80 parts by mass, more preferably 25 to 60 parts by mass, and even more preferably 25 to 45 parts by mass, when the total mass of the silicon carbide powder and metal silicon powder is 100 parts by mass. The average particle size of the silicon carbide particles in the silicon carbide powder is preferably 3 to 50 μm, more preferably 3 to 40 μm. The average particle size of the metal silicon particles in the metal silicon powder is preferably 2 to 35 μm, more preferably 2 to 25 μm. The average particle sizes of the silicon carbide particles and metal silicon particles refer to the arithmetic mean diameter on a volume basis when the particle size frequency distribution is measured by laser diffraction. The silicon carbide particles are fine particles of silicon carbide that constitute the silicon carbide powder, and the metal silicon particles are fine particles of metal silicon that constitute the metal silicon powder.

[0066] The content of water in the forming raw material is, for example, preferably 20 to 60 parts by mass, and more preferably 25 to 50 parts by mass, when the total mass of the silicon carbide powder and the metallic silicon powder is 100 parts by mass.

[0067] In step 1, the forming raw materials are kneaded to prepare a clay. Any appropriate device or mechanism can be used as the kneading means. Specific examples include a kneader and a vacuum clay kneader.

[0068] The forming raw material may contain a binder, a surfactant, and a pore former in addition to the silicon carbide powder and the silicon powder.

[0069] Examples of binders include methyl cellulose, hydroxypropyl methyl cellulose, hydroxypropoxyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, and polyvinyl alcohol. Among these, it is preferable to use methyl cellulose and hydroxypropoxyl cellulose in combination. The content of the binder is preferably 2.0 to 10.0 parts by mass when the total mass of the silicon carbide powder and the silicon powder is 100 parts by mass.

[0070] Examples of surfactants that can be used include ethylene glycol, dextrin, fatty acid soap, and polyalcohol. These may be used alone or in combination of two or more. The content of the surfactant is preferably 0.1 to 2.0 parts by mass when the total mass of the silicon carbide powder and the silicon powder is 100 parts by mass.

[0071] The pore-forming material is not particularly limited as long as it forms pores after firing, and examples thereof include graphite, starch, foamed resin, water-absorbent resin, silica gel, etc. The content of the pore-forming material is preferably 0.5 to 10.0 parts by mass when the total mass of the silicon carbide powder and silicon powder is 100 parts by mass. The average particle diameter of the pore-forming material is preferably 10 to 30 μm. The average particle diameter of the pore-forming material refers to the arithmetic mean diameter on a volume basis when the frequency distribution of particle size is measured by laser diffraction. When the pore-forming material is a water-absorbent resin, the average particle diameter of the pore-forming material refers to the average particle diameter after water absorption.

[0072] (Step 2) In step 2, the clay produced in step 1 is molded to obtain a honeycomb molded body. Specifically, the clay is extrusion molded to produce a columnar honeycomb molded body having an outer peripheral wall and partition walls. A die having the desired overall shape, cell shape, partition wall thickness, cell density, etc. can be used during extrusion molding. Next, it is preferable to dry the obtained honeycomb molded body. If the length of the honeycomb molded body in the cell extension direction is not the desired length, both ends of the honeycomb molded body can be cut to obtain the desired length. The honeycomb molded body after drying is called a dried honeycomb body.

[0073] The honeycomb formed body may be fired once as a modification of step 2. That is, in this modification, the honeycomb formed body is fired to prepare a honeycomb fired body, and step 3 is then carried out on the honeycomb fired body.

[0074] (Step 3) Step 3 is a step of applying a pair of electrode layer forming pastes to the outer surface of the peripheral wall of the honeycomb formed body so that the pastes extend in bands in the cell extension direction across the central axis of the honeycomb formed body, thereby producing a honeycomb formed body with electrode layer forming pastes. The electrode layer forming paste can be formed by appropriately adding various additives to raw material powders (metal powders, ceramic powders, etc.) blended according to the required characteristics of the electrode layer, and kneading the mixture. The average particle diameter of the raw material powders is not limited, but is preferably, for example, 5 to 50 μm, and more preferably 10 to 30 μm. The average particle diameter of the raw material powder refers to the arithmetic mean diameter on a volume basis when the particle size frequency distribution is measured by laser diffraction.

[0075] Next, the obtained electrode layer forming paste is applied to required locations on the outer surface of the peripheral wall of a honeycomb formed body (typically a dried honeycomb body) to obtain a honeycomb formed body with the electrode layer forming paste. The method of preparing the electrode layer forming paste and the method of applying the electrode layer forming paste to the honeycomb formed body can be performed in accordance with known methods for manufacturing honeycomb structures. However, in order to give the electrode layer a lower volume resistivity than the peripheral wall and partition walls, the metal content can be made higher than that of the peripheral wall and partition walls, or the particle size of the metal particles in the raw material powder can be made smaller. After application, it is preferable to dry the electrode layer forming paste.

[0076] (Step 4) Step 4 is a step of firing the honeycomb formed body with the electrode layer forming paste to obtain a honeycomb fired body, i.e., the desired honeycomb structure. Before firing, degreasing may be performed to remove binders and the like. The degreasing and firing methods are not particularly limited, and firing can be performed using an electric furnace, a gas furnace, or the like. Firing conditions vary depending on the material of the honeycomb structure, but preferably involve heating at 1400 to 1500°C for 1 to 20 hours in an inert atmosphere such as nitrogen or argon.

[0077] An electrically heated carrier can be manufactured by joining a metal terminal to the electrode layer of the honeycomb structure obtained in this manner. The joining method is not particularly limited, but examples thereof include thermal spraying, welding, and brazing. In order to improve the bonding between the electrode layer and the metal terminal, a base layer may be formed by a method such as thermal spraying.

[0078] An appropriate catalyst may be supported on the electrically heated carrier depending on the application. As a method for supporting a catalyst on a honeycomb structure, for example, a catalyst slurry is introduced into cells by a conventionally known suction method or the like, and is allowed to adhere to the surfaces and pores of the partition walls, and then high-temperature treatment is performed to bake the catalyst contained in the catalyst slurry onto the partition walls and support the catalyst.

[0079] The following examples are provided to provide a better understanding of the present invention and its advantages, but the present invention is not limited to these examples.

[0080] Example 1 (1. Preparation of Cylindrical Puddle) 30 g of phosphate ester salt and 12.5 g of boric acid were added to 30 kg of pure water and stirred for 20 minutes to obtain an aqueous solution containing P and B. Next, Al- and N-doped silicon carbide (SiC) powder and silicon (Si) powder were mixed in a mass ratio of 65:35 to prepare a ceramic raw material. The amount of Al and N doped into SiC (silicon carbide) was adjusted by mixing SiC (silicon carbide) with different amounts of Al and N doped. Hydroxypropyl methylcellulose as a binder and a water-absorbent resin as a pore-forming material were added to this ceramic raw material, and the aforementioned aqueous solution containing P and B was added to obtain a molding raw material. Next, the molding raw material was kneaded using a vacuum kneader to prepare a cylindrical moldable clay.

[0081] In the molding raw material, the content of the binder was 7 parts by mass when the total of the silicon carbide (SiC) powder and the silicon (Si) powder was 100 parts by mass. The content of the pore-forming material was 3 parts by mass when the total of the silicon carbide (SiC) powder and the silicon (Si) powder was 100 parts by mass. The content of the aqueous solution was 30 parts by mass when the total of the silicon carbide (SiC) powder and the silicon (Si) powder was 100 parts by mass. The average particle diameter of the silicon carbide powder was 20 μm, and the average particle diameter of the silicon powder was 6 μm. The average particle diameter of the pore-forming material was 20 μm. The average particle diameters of the silicon carbide powder, the silicon powder, and the pore-forming material refer to the arithmetic mean diameter on a volume basis when the particle size frequency distribution is measured by a laser diffraction method.

[0082] (2. Production of dried honeycomb body) The obtained cylindrical clay was molded using an extrusion molding machine with a predetermined die structure to obtain a cylindrical honeycomb molded body in which each cell shape in a cross section perpendicular to the cell extension direction is hexagonal. This honeycomb molded body was dried by high-frequency dielectric heating, and then further dried in an air atmosphere at 120°C for 2 hours using a hot air dryer, and both end faces were cut by a predetermined amount to produce a dried honeycomb body.

[0083] (3. Preparation of electrode layer forming paste) Silicon (Si) powder, silicon carbide (SiC) powder, methyl cellulose, glycerin, and water were mixed using a planetary centrifugal mixer to prepare an electrode layer forming paste. The Si powder and SiC powder were blended at a volume ratio of Si powder:SiC powder = 40:60. Furthermore, when the total of the Si powder and SiC powder was 100 parts by mass, the amount of methyl cellulose was 0.5 parts by mass, the amount of glycerin was 10 parts by mass, and the amount of water was 38 parts by mass. The average particle diameter of the silicon powder was 6 μm. The average particle diameter of the silicon carbide powder was 35 μm. These average particle diameters refer to the arithmetic mean diameter on a volume basis when the particle size frequency distribution was measured by laser diffraction.

[0084] (4. Application of electrode layer forming paste) The electrode layer forming paste was applied to two locations on the outer surface of the outer wall of the dried honeycomb body using a curved surface printing machine, facing each other across the central axis. Each application area was formed in a band shape over the entire length between both end faces of the dried honeycomb body (angle θ = 180°, central angle α = 127°). Next, the electrode layer forming paste applied to the dried honeycomb body was dried to obtain a dried honeycomb body with the electrode layer forming paste. The drying temperature was 70°C.

[0085] (5. Firing) The obtained dried honeycomb body with the electrode layer forming paste was degreased in an air atmosphere at 550°C for 3 hours. Next, the degreased dried honeycomb body was fired in an argon atmosphere at 1450°C for 2 hours to obtain a cylindrical honeycomb structure. The honeycomb structures were manufactured in the number required for the following tests.

[0086] (6. Specifications of honeycomb structure) The honeycomb structure obtained above had a circular end face with a diameter of 80 mm, a height (length in the cell extension direction) of 80 mm, a partition wall thickness of 125 mm, a peripheral wall thickness of 0.5 mm, and a cell density of 90 cells / cm 2 The porosity of the partition walls was 38%.

[0087] (7. Contents of Si, SiC, and SiO2) The contents of Si (silicon), SiC (silicon carbide), and SiO2 (silicon oxide) in the ceramics constituting the honeycomb structure part of the honeycomb structure obtained above were measured according to the method described above. The results are shown in Table 1.

[0088] (8. Dopant Concentration in Silicon) The P concentration and B concentration in silicon (Si) in the ceramics constituting the honeycomb structure portion of the honeycomb structure obtained above were measured according to the method described above. The ICP (inductively coupled plasma) analyzer used was a PS3510DD model manufactured by Hitachi High-Technologies Corporation. The results are shown in Table 1.

[0089] (9. Dopant Concentration in Silicon Carbide) The Al concentration and N concentration in silicon carbide (SiC) in the ceramic constituting the honeycomb structure portion of the honeycomb structure obtained above were measured according to the method described above. An SEM model S-3400N manufactured by Hitachi High-Tech Corporation was used, and a SIMS model NanoSIMS 50L manufactured by CAMECA was used. The results are shown in Table 1.

[0090] (10. Measurement of Volume Resistivity) The volume resistivity of the honeycomb structure portion of the honeycomb structure obtained above was measured at 25° C. according to the method described above. The results are shown in Table 1.

[0091] (11. NTC thermistor characteristics: ρ v500 / ρ v50 ) Volume resistivity (ρ v50 ) versus volume resistivity at 500 ° C. (ρ v500 ) ratio (ρ v500 / ρ v50 The results are shown in Table 1.

[0092] (12. Porosity) A partition wall sample was taken from the honeycomb structure portion of the honeycomb structure obtained above, and the porosity was measured using a mercury porosimeter. The results are shown in Table 1.

[0093] (13. Heat Generation Distribution) When a voltage of 400 V was applied to the center of the surface of each of the pair of electrode layers of the honeycomb structure obtained above for 20 seconds, the temperature distribution at both end faces and the outer wall of the honeycomb structure was observed by thermography, and the uniformity of the heat generation distribution was evaluated. The evaluation criteria were as follows. The results are shown in Table 1. A: When electricity was applied to the honeycomb structure, the difference between the maximum and minimum temperatures was within +150°C compared to the difference between the maximum and minimum temperatures in Example 1. B: When electricity was applied to the honeycomb structure, the difference between the maximum and minimum temperatures was more than +150°C but within +250°C compared to the difference between the maximum and minimum temperatures in Example 1. C: When electricity was applied to the honeycomb structure, the difference between the maximum and minimum temperatures was more than +250°C compared to the difference between the maximum and minimum temperatures in Example 1, raising concerns about the impact on cracks.

[0094] Examples 2 and 3 The compounding ratio of silicon carbide (SiC) powder and silicon (Si) powder in the forming raw material was changed so that the contents of Si (silicon), SiC (silicon carbide), and SiO2 (silicon oxide) in the ceramics constituting the honeycomb structure portion of the honeycomb structure were the values ​​shown in Table 1. In addition, the concentrations of P and B in the aqueous solution containing P and B were adjusted so that the B concentration and P concentration in Si were the same as in Example 1. Otherwise, honeycomb structures were produced in the same manner as in Example 1. The obtained honeycomb structures were subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0095] Example 4 A honeycomb structure was produced in the same manner as in Example 2, except that the amounts of P and B doped into Si (silicon) were changed by changing the concentrations of P and B in the aqueous solution containing P and B. The obtained honeycomb structure was subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0096] Examples 5, 6, and 8 Honeycomb structures were fabricated in the same manner as in Example 1, except that the amounts of P and B doped into Si (silicon) were changed by changing the concentrations of P and B in the aqueous solution containing P and B. The obtained honeycomb structures were subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0097] Example 7 The compounding ratio of silicon carbide (SiC) powder and silicon (Si) powder in the forming raw material was changed so that the contents of Si (silicon), SiC (silicon carbide), and SiO2 (silicon oxide) in the ceramics constituting the honeycomb structure portion of the honeycomb structure were the values ​​shown in Table 1. In addition, the concentrations of P and B in the aqueous solution containing P and B were adjusted so that the B concentration and P concentration in Si were the same as in Example 6. Otherwise, a honeycomb structure was produced in the same manner as in Example 6. The obtained honeycomb structure was subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0098] Example 9 A honeycomb structure was fabricated in the same manner as in Example 3, except that the amounts of P and B doped into Si (silicon) were changed by changing the concentrations of P and B in the aqueous solution containing P and B. The obtained honeycomb structure was subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0099] Example 10 A honeycomb structure was produced in the same manner as in Example 2, except that the amounts of Al and N doped into SiC (silicon carbide) were changed by mixing SiC (silicon carbide) with different doping amounts of Al and N. The obtained honeycomb structure was subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0100] Examples 11 to 18 Honeycomb structures were produced in the same manner as in Example 1, except that the amounts of Al and N doped into SiC (silicon carbide) were changed by mixing SiC (silicon carbide) with different doping amounts of Al and N. The obtained honeycomb structures were subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0101] Comparative Example 1 A honeycomb structure was produced in the same manner as in Example 1, except that the amounts of P and B doped into Si (silicon) were changed by changing the concentrations of P and B in an aqueous solution containing P and B, and the amounts of Al and N doped into SiC (silicon carbide) were changed by mixing SiC (silicon carbide) with different doping amounts of Al and N. The obtained honeycomb structure was subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0102] Comparative Example 2 The compounding ratio of silicon carbide (SiC) powder and silicon (Si) powder in the raw materials was changed so that the contents of Si (silicon), SiC (silicon carbide), and SiO2 (silicon oxide) in the ceramics constituting the honeycomb structure portion of the honeycomb structure were the values ​​shown in Table 1. The amounts of P and B doped into Si (silicon) were changed by changing the concentrations of P and B in an aqueous solution containing P and B, and the amounts of Al and N doped into SiC (silicon carbide) were changed by mixing SiC (silicon carbide) with different doping amounts of Al and N. A honeycomb structure was otherwise fabricated in the same manner as in Example 1. The obtained honeycomb structure was subjected to the same characteristic evaluation as in Example 1. The results are shown in Table 1.

[0103]

[0104] As can be seen from the above examples and comparative examples, by appropriately controlling the silicon carbide and silicon contents, P-B content, and Al-N content in the ceramics constituting the honeycomb structure portion, the NTC thermistor characteristics are alleviated, and the uniformity of the heat generation distribution of the honeycomb structure is significantly improved.

[0105] 100: Electrically heated carrier 110: Honeycomb structure 112a: First electrode layer 112b: Second electrode layer 113: Partition wall 114: Outer wall 115: Cell 116: First end face 118: Second end face 120: Base layer 130: Metal terminal 200: Exhaust gas purification device 220: Metal tube 240: Electric wire

Claims

1. A honeycomb structure comprising: a ceramic honeycomb structure having an outer peripheral wall, and partition walls disposed inside the outer peripheral wall to separate a plurality of cells forming a fluid flow path from a first end face to a second end face, and a pair of electrode layers provided on the outer surface of the outer peripheral wall, extending in a band shape in the extension direction of the cells, and disposed so as to face each other across the central axis of the honeycomb structure, wherein the ceramic contains at least silicon and silicon carbide, and satisfies one or both of the following conditions (1) and (2): (1) The silicon content in the ceramic is 21 to 30 mass%, the silicon contains P and B, and the value obtained by subtracting the B concentration from the P concentration in the silicon (P-B amount) is 20 mass ppm or more. (2) The ceramic has a silicon carbide content of 50 mass% or more, the silicon carbide contains Al and N, and the value obtained by subtracting the N concentration from the Al concentration in the silicon carbide (Al-N amount) is 130 ppm by mass or more and 450 ppm by mass or less.

2. A honeycomb structure according to claim 1, which satisfies both of the conditions (1) and (2).

3. The honeycomb structure according to claim 1 or 2, wherein the ceramic satisfies one or both of the following conditions (3) and (4): (3) The silicon content in the ceramic is 21 to 30 mass%, the silicon contains P and B, and the value obtained by subtracting the B concentration from the P concentration in the silicon (P-B amount) is 20 mass ppm or more. (4) The silicon carbide content in the ceramic is 50 mass % or more, the silicon carbide contains Al and N, and the value obtained by subtracting the N concentration from the Al concentration in the silicon carbide (Al-N amount) is 300 mass ppm or more and 450 mass ppm or less.

4. A honeycomb structure according to claim 3, which satisfies both of the conditions (3) and (4).

5. The honeycomb structure according to claim 1 or 2, wherein the total content of silicon and silicon carbide in said ceramic is 80 to 95 mass %.

6. The honeycomb structure according to claim 1 or 2, wherein the ceramic further contains 5 to 20 mass % of silicon oxide.

7. A honeycomb structure according to claim 1 or 2, wherein the partition walls of said honeycomb structure portion have a porosity of 30% or more.

8. The volume resistivity (ρ v50 ) versus volume resistivity at 500°C (ρ v500 ) ratio (ρ v500 / ρ v50 3. The honeycomb structure according to claim 1, wherein the ratio of the surface roughness to the surface roughness is 0.30 to 0.

80.

9. An electrically heated carrier comprising: the honeycomb structure according to claim 1 or 2; and metal terminals joined to the outer surfaces of the pair of electrode layers, respectively.

10. An exhaust gas purification device comprising: an electrically heated carrier according to claim 9; and a metal tube that houses the electrically heated carrier.

Citation Information

Patent Citations

  • Method for producing conductive ceramic sintered compact

    JP2012214306A

  • Honey-comb structure and electric heating carrier

    JP2022142543A