Polymer dispersion-type liquid crystal film
The PDLC film addresses the low transparency issue in conventional PDLC films by optimizing the particle diameter and weight ratio of the liquid crystal component and dichroic dye, achieving high clarity and low haze in the colored state, thus enhancing its applicability in transparent and colored states.
Patent Information
- Application Number
- PCT/JP2024/008798
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-07
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional polymer dispersed liquid crystal (PDLC) films using dichroic dyes tend to have low transparency in the colored state, which limits their application in scenarios requiring high transparency and clear visibility.
A PDLC film structure comprising a polymer matrix with droplets of a liquid crystal component and dichroic dye, where the average particle diameter is 1 μm or less, and a weight ratio of polymer matrix to liquid crystal component and dichroic dye is optimized to achieve high clarity and low haze in the colored state, allowing for switching between colored and transparent states while maintaining improved transparency.
The PDLC film achieves high clarity and low haze in the colored state, enabling clear visibility and efficient light transmittance, making it suitable for applications such as smart windows and displays.
Smart Images

Figure JP2024008798_03102024_PF_FP_ABST
Abstract
Description
Polymer dispersed liquid crystal film
[0001] The present invention relates to a polymer dispersed liquid crystal film.
[0002] A PDLC film having a polymer dispersed liquid crystal (PDLC) layer containing a polymer matrix and liquid crystal droplets between a pair of transparent electrode layers can change the degree of scattering of light transmitted through the PDLC layer depending on the amount of applied voltage. For example, a PDLC film can switch between a light scattering state (scattering state) and a light transmitting state (transparent state) by switching between an applied voltage state and an unapplied voltage state (Patent Document 1). Taking advantage of this function, PDLC films are being increasingly applied to windows, walls, partitions, and the like in vehicles such as cars and trains, offices, commercial facilities, and residences as light control films that can improve privacy or security.
[0003] In the above-mentioned PDLC film, when a dichroic dye is contained in the liquid crystal component droplets, it is possible to switch between a colored state in which light of at least some wavelengths is absorbed and a transparent state in which light is transmitted by switching between a voltage-applied state and a voltage-unapplied state (Patent Document 2).
[0004] JP 2002-189123 A International Publication No. 2022 / 186062
[0005] PDLC films using conventional dichroic dyes tend to have low transparency in the colored state. Therefore, in applications where transparency and clear visibility are required, there is a demand for PDLC films with improved transparency in the colored state.
[0006] The present invention has been made to solve the above-mentioned problems, and its main object is to provide a PDLC film that can be switched between a colored state and a transparent state and has improved transparency in the colored state.
[0007] [1] According to one aspect of the present invention, there is provided a polymer dispersed liquid crystal film comprising, in this order, a first transparent conductive film, a polymer dispersed liquid crystal layer, and a second transparent conductive film, wherein the polymer dispersed liquid crystal layer comprises a polymer matrix and droplets dispersed in the polymer matrix, the droplets comprising a liquid crystal component and a dichroic dye, the droplets having an average particle size of 1 μm or less and a clarity in a colored state of 90 or more. [2] In the polymer dispersed liquid crystal film according to [1] above, the droplets may have an average particle size of 0.01 μm or more and less than 0.38 μm. [3] In the polymer dispersed liquid crystal film according to [1] or [2] above, the liquid crystal component may have a birefringence of 0.25 or less. [4] In the polymer dispersed liquid crystal film according to any one of [1] to [3] above, the weight ratio (former:latter) of the content of the polymer matrix to the total content of the liquid crystal component and the dichroic dye in the polymer dispersed liquid crystal layer may be 10:90 to 70:30. [5] In the polymer dispersed liquid crystal film according to any one of [1] to [4] above, the thickness of the polymer dispersed liquid crystal layer may be 30 μm or less. [6] In the polymer dispersed liquid crystal film according to any one of [1] to [5] above, the total light transmittance in the colored state may be 50% or less. [7] In the polymer dispersed liquid crystal film according to any one of [1] to [6] above, the haze in the colored state may be 80% or less.
[0008] SUMMARY OF THE INVENTION According to embodiments of the present invention, a PDLC film is provided that is switchable between a colored state and a transparent state and has improved transparency in the colored state.
[0009] 1 is a schematic cross-sectional view of a PDLC film in one embodiment of the present invention.
[0010] Preferred embodiments of the present invention will be described below, but the present invention is not limited to these embodiments. In this specification, the term "to" indicating a range of values includes the upper and lower limits.
[0011] A. Polymer-Dispersed Liquid Crystal Film A polymer-dispersed liquid crystal film according to an embodiment of the present invention comprises, in this order, a first transparent conductive film, a polymer-dispersed liquid crystal layer, and a second transparent conductive film, wherein the polymer-dispersed liquid crystal layer comprises a polymer matrix and droplets (hereinafter sometimes referred to as "liquid crystal droplets") dispersed in the polymer matrix and containing a liquid crystal component and a dichroic dye, the droplets having an average particle size of 1 μm or less and a clarity of 90 or more in a colored state.
[0012] As described above, the appearance of the PDLC film changes depending on the applied voltage. In one embodiment, the PDLC film is transparent when a voltage is applied and colored when no voltage is applied (normal mode). In another embodiment, the PDLC film is colored when a voltage is applied and transparent when no voltage is applied (reverse mode).
[0013] FIG. 1 is a schematic cross-sectional view illustrating the configuration of an example of a normal-mode PDLC film according to an embodiment of the present invention. FIG. 1( a) illustrates a state in which no voltage is applied to the PDLC layer (colored state), and FIG. 1( b) illustrates a state in which a voltage is applied to the PDLC layer (transparent state). The PDLC film 100 includes, in this order, a first transparent conductive film 10, a PDLC layer 20 including a polymer matrix 22 and liquid crystal droplets 25 dispersed in the polymer matrix 22, and a second transparent conductive film 30. The liquid crystal droplets 25 are so-called guest-host liquid crystals containing a liquid crystal component 23 and a dichroic dye 24. As shown in FIG. 1( a), when no voltage is applied, the liquid crystal component 23 and the dichroic dye 24 in the liquid crystal droplets 25 are misaligned, and light is absorbed by the dichroic dye 24, resulting in the PDLC film 100 being colored. 1(b), when a voltage is applied, the liquid crystal component 23 is oriented along the electric field direction, and the dichroic dye 24 is also oriented following the liquid crystal component 23. As a result, the refractive index of the liquid crystal droplets 25 and the refractive index of the polymer matrix 22 become the same, and the PDLC film 100 becomes transparent.
[0014] Although not shown, in a reverse mode PDLC film, an alignment film is provided on the surface of the transparent conductive film, so that when no voltage is applied, the liquid crystal component 23 and dichroic dye 24 in the liquid crystal droplets 25 are aligned to form a transparent state, and when a voltage is applied, the alignment state of the liquid crystal component 23 and dichroic dye 24 changes, resulting in a colored state.
[0015] The clarity of the PDLC film in the colored state is, for example, 90 or more, preferably 92 or more, more preferably 95 or more, and even more preferably 97 or more. The upper limit of clarity is 100. Clarity corresponds to the narrow-angle scattering degree, and is the transmittance in an angular range of ±2.5° relative to the direction of travel of parallel light incident on the PDLC film. High clarity means that the boundary of an image viewed through the PDLC film is clear. Clarity is expressed as the amount of light L of light that, among the light transmitted through the PDLC film, travels straight along the optical axis of the parallel light incident on the PDLC film. C The amount of narrow-angle scattered light whose angle with respect to the optical axis of the parallel light is within ±2.5° is defined as the light amount L R When the above formula is used, it is calculated by the following formula (1): 100 × (L C -L R ) / (L C +L R ) … Formula (1)
[0016] The total light transmittance of the PDLC film in the colored state may be, for example, 50% or less, 40% or less, 30% or less, 20% or less, or 10% or less, and may be, for example, 0.5% or more, or 1% or more. The total light transmittance of the PDLC film in the transparent state may be, for example, 15% or more, 20% or more, 30% or more, or 50% or more, and may be, for example, 99% or less. The difference in total light transmittance between the transparent and colored states of the PDLC film may be, for example, 10% or more, 20% or more, or 30% or more. The total light transmittance may be measured in accordance with JIS K 7361.
[0017] The haze of the PDLC film in the colored state is, for example, 80% or less, and may be 60% or less, 50% or less, or 45% or less, and may be, for example, 5% or more. The haze of the PDLC film in the transparent state is, for example, 30% or less, and may be 20% or less, 10% or less, or 5% or less, and may be, for example, 0.1% or more. The difference in haze between the transparent and colored states of the PDLC film is, for example, 10% or more, and may be 20% or more, 30% or more, or 40% or more. Haze can be measured in accordance with JIS K 7136.
[0018] The voltage applied to the PDLC film during voltage application is a voltage capable of operating the PDLC film (operating voltage), and may be, for example, 5 V to 300 V, and preferably 10 V to 200 V. In this specification, "when a voltage is applied" refers to a state in which an operating voltage is applied to the PDLC film, and may be, for example, a state in which a voltage of 150 V is applied.
[0019] The total thickness of the PDLC film is, for example, 30 μm to 250 μm, preferably 50 μm to 150 μm.
[0020] A-1. First Transparent Conductive Film The first transparent conductive film 10 typically includes a first transparent substrate 12 and a first transparent electrode layer 14 provided on one side thereof (the PDLC layer 20 side). The first transparent conductive film 10 may optionally include a hard coat layer on one or both sides of the first transparent substrate 12, and may also include a refractive index adjusting layer between the first transparent substrate 12 and the first transparent electrode layer 14.
[0021] The surface resistance value of the first transparent conductive film is preferably 1 Ω / □ to 1000 Ω / □, more preferably 5 Ω / □ to 300 Ω / □, and even more preferably 10 Ω / □ to 200 Ω / □.
[0022] The haze value of the first transparent conductive film is preferably 20% or less, more preferably 10% or less, and even more preferably 0.1% to 10%.
[0023] The total light transmittance of the first transparent conductive film is preferably 40% or more, more preferably 60% or more, and even more preferably 80% or more.
[0024] The first transparent substrate can be formed using any appropriate material. Typically, the first transparent substrate is a polymer film primarily composed of a thermoplastic resin. Examples of thermoplastic resins include polyester-based resins; cycloolefin-based resins such as polynorbornene; acrylic resins; polycarbonate-based resins; and cellulose-based resins. Among these, polyester-based resins, cycloolefin-based resins, and acrylic resins are preferred. These resins are excellent in transparency, mechanical strength, thermal stability, moisture-blocking properties, and the like. The thermoplastic resins may be used alone or in combination of two or more. Optical films used in polarizing plates, such as low-retardation substrates, high-retardation substrates, retardation plates, absorptive polarizing films, and polarized selective reflection films, can also be used as the first transparent substrate.
[0025] The thickness of the first transparent substrate is preferably 200 μm or less, more preferably 3 μm to 100 μm, and even more preferably 5 μm to 70 μm. By setting the thickness of the first transparent substrate to 200 μm or less, the function of the PDLC layer can be fully exhibited.
[0026] The total light transmittance of the first transparent substrate is preferably 40% or more, more preferably 60% or more, and even more preferably 80% or more.
[0027] The first transparent electrode layer may be made of, for example, indium tin oxide (ITO), zinc oxide (ZnO), or tin oxide (SnO 2 The first transparent electrode layer may be formed using a metal oxide such as ZnO. In this case, the metal oxide may be an amorphous metal oxide or a crystallized metal oxide. The first transparent electrode layer may also be formed using metal nanowires such as silver nanowires (AgNW), carbon nanotubes (CNT), an organic conductive film, a metal layer, or a laminate thereof. Preferably, a transparent electrode layer containing ITO is formed. A transparent electrode layer containing ITO has excellent transparency. The first transparent electrode layer may be patterned into a desired shape depending on the purpose.
[0028] The total light transmittance of the first transparent electrode layer is preferably 85% or more, more preferably 87% or more, and even more preferably 90% or more. By using a transparent electrode layer having a total light transmittance in this range, a PDLC film having a high total light transmittance in the transparent state can be obtained. The higher the total light transmittance, the more preferable it is, and the upper limit is, for example, 99%.
[0029] The thickness of the first transparent electrode layer is, for example, 10 nm or more, preferably 15 nm or more, and for example, 50 nm or less, preferably 35 nm or less, more preferably 30 nm or less.
[0030] The first transparent electrode layer is formed on one surface of the first transparent substrate by, for example, sputtering. After forming the metal oxide layer by sputtering, it can be crystallized by annealing. Annealing is performed by, for example, heat treatment at 120°C to 300°C for 10 to 120 minutes.
[0031] The refractive index adjusting layer and the hard coat layer may have a structure well known in the art, and therefore detailed description of their structures will be omitted.
[0032] A-2. Polymer-Dispersed Liquid Crystal Layer The PDLC layer 20 includes a polymer matrix 22 and liquid crystal droplets 25 dispersed in the polymer matrix 22. The average particle size of the liquid crystal droplets is typically 1 μm or less, for example, 0.5 μm or less. A PDLC layer containing liquid crystal droplets with a small particle size exhibits low scattering properties, and therefore, by setting the average particle size of the liquid crystal droplets to 1 μm or less, a PDLC film with high clarity can be obtained. From the perspective of further reducing scattering properties, the average particle size of the liquid crystal droplets is preferably equal to or less than the wavelength of visible light. Specifically, the average particle size of the liquid crystal droplets is preferably less than 0.38 μm, more preferably less than 0.3 μm, even more preferably less than 0.2 μm, even more preferably 0.18 μm or less, even more preferably 0.15 μm or less, and even more preferably 0.12 μm or less. The lower limit of the average particle size of the liquid crystal droplets is not limited as long as the effects of the present invention are obtained, and may be, for example, 0.01 μm or more or 0.05 μm or more. The average particle size of the liquid crystal droplets is a volume average particle size, and can be determined, for example, by the method described in the Examples.
[0033] The particle diameter of the liquid crystal droplets preferably has a relatively narrow particle size distribution. The coefficient of variation (CV value) of the particle diameter of the liquid crystal droplets may be, for example, less than 0.4, preferably 0.35 or less, and more preferably 0.3 or less. The coefficient of variation can be calculated using the following formula: CV value = standard deviation of particle diameter distribution of liquid crystal droplets / average particle diameter
[0034] The polymer matrix may be composed of any appropriate resin. The resin for forming the polymer matrix may be appropriately selected depending on the light transmittance, the refractive index of the liquid crystal component, the adhesion to the transparent conductive film, etc. The resin for forming the polymer matrix preferably has a refractive index similar to that of the liquid crystal component.
[0035] Specific examples of the polymer matrix-forming resin include urethane resins, polyvinyl alcohol resins, polyethylene resins, polypropylene resins, and acrylic resins. These are preferably water-soluble or water-dispersible resins. Only one type of polymer matrix-forming resin may be used, or two or more types may be used in combination.
[0036] As the liquid crystal component, any appropriate liquid crystal compound can be used alone or in combination. The birefringence (Δn=ne-no; ne is the extraordinary refractive index, no is the ordinary refractive index) of the liquid crystal component at a wavelength of 589 nm is, for example, 0.25 or less. From the viewpoint of obtaining a PDLC film with high clarity, the birefringence is preferably 0.2 or less, more preferably 0.15 or less, for example, 0.12 or less, or may be, for example, 0.1 or less. The birefringence is, for example, 0.01 or more, 0.05 or more, or 0.08 or more. By using a liquid crystal component having the above birefringence, the scattering property of the PDLC layer in a colored state (e.g., when no voltage is applied) can be reduced, resulting in a PDLC film with high clarity.
[0037] The dielectric anisotropy of the liquid crystal component may be positive or negative. The liquid crystal component may be, for example, a nematic liquid crystal, a smectic liquid crystal, or a cholesteric liquid crystal. Nematic liquid crystals are preferred because they can achieve excellent transparency in the transparent state.
[0038] Examples of nematic liquid crystal compounds include biphenyl-based compounds, phenylbenzoate-based compounds, cyclohexylbenzene-based compounds, azoxybenzene-based compounds, azobenzene-based compounds, azomethine-based compounds, terphenyl-based compounds, biphenylbenzoate-based compounds, cyclohexylbiphenyl-based compounds, phenylpyridine-based compounds, cyclohexylpyrimidine-based compounds, cholesterol-based compounds, and fluorine-based compounds.
[0039] As the dichroic dye, any appropriate dichroic dye that is compatible with the liquid crystal component can be used. The dichroic dye may have a positive Δε or a negative Δε. The dichroic dye itself may exhibit liquid crystallinity. The dichroic dye may be used alone or in combination of two or more.
[0040] Specific examples of dichroic dyes include azo dyes, anthraquinone dyes, naphthoquinone dyes, perylene dyes, quinophthalone dyes, tetrazine dyes, and benzothiadiazole dyes. Among these, from the viewpoints of absorption coefficient, solubility in liquid crystal components, light resistance, and the like, it is preferable that the dichroic dye contains an anthraquinone dye or an azo dye. For example, the azo dyes, anthraquinone dyes, or mixtures thereof described in "Liquid Crystal Device Handbook," edited by Committee 142 of the Japan Society for the Promotion of Science, published by the Japan Industrial Newspaper Co., Ltd. (1989), pages 192 to 196 and 724 to 730, can be used. Various dichroic dyes are commercially available, and these can be used as appropriate.
[0041] The PDLC layer may further contain any appropriate component as needed, such as a surfactant, a leveling agent, a crosslinking agent, a dispersion stabilizer, etc.
[0042] The content of the liquid crystal component in the PDLC layer is, for example, 30 to 90% by weight, preferably 35 to 85% by weight, and more preferably 40 to 80% by weight.
[0043] The content of the dichroic dye in the PDLC layer is, for example, 0.1 to 20 parts by weight, preferably 1 to 15 parts by weight, and more preferably 3 to 10 parts by weight, per 100 parts by weight of the liquid crystal component.
[0044] The weight ratio (former:latter) of the content of the polymer matrix to the total content of the liquid crystal component and the dichroic dye in the PDLC layer is, for example, 10:90 to 70:30, preferably 15:85 to 65:35, and more preferably 20:80 to 60:40.
[0045] The total content of the polymer matrix, liquid crystal component, and dichroic dye in the PDLC layer is, for example, 80% by weight or more, preferably 90% by weight or more, more preferably 95% by weight or more, and is, for example, 100% by weight or less, preferably 99% by weight or less.
[0046] The thickness of the PDLC layer is preferably 40 μm or less, more preferably 30 μm or less, for example, 25 μm or less, or for example, 20 μm or less, and is preferably 2 μm or more, more preferably 3 μm or more, for example, 5 μm or more, or for example, 10 μm or more. When the thickness of the PDLC layer is within the above range, a PDLC film with high clarity and high colorability can be suitably obtained.
[0047] A-3. Second Transparent Conductive Film The second transparent conductive film 30 typically includes a second transparent substrate 32 and a second transparent electrode layer 34 provided on one side thereof (the PDLC layer 20 side). The second transparent conductive film 30 may optionally include a hard coat layer on one or both sides of the second transparent substrate 32, and may also include a refractive index adjusting layer between the second transparent substrate 32 and the second transparent electrode layer 34.
[0048] The surface resistance value of the second transparent conductive film is preferably 1 Ω / □ to 1000 Ω / □, more preferably 5 Ω / □ to 300 Ω / □, and even more preferably 10 Ω / □ to 200 Ω / □.
[0049] The haze value of the second transparent conductive film is preferably 20% or less, more preferably 10% or less, and even more preferably 0.1% to 10%.
[0050] The total light transmittance of the second transparent conductive film is preferably 40% or more, more preferably 60% or more, and even more preferably 80% or more.
[0051] The second transparent substrate and the second transparent electrode layer can be described in the same manner as the first transparent substrate and the first transparent electrode layer, respectively. The second transparent conductive film may have the same configuration as the first transparent conductive film, or may have a different configuration.
[0052] B. Method for Producing Polymer-Dispersed Liquid Crystal Film The PDLC film described in Section A can be produced by any appropriate production method. The method for producing the PDLC film described in Section A includes, for example, mixing a liquid crystal component, a dichroic dye, and a dispersion medium to prepare a liquid crystal emulsion containing particles containing the liquid crystal component and the dichroic dye (Step A), mixing the liquid crystal emulsion with a polymer matrix-forming resin to prepare a coating liquid containing the particles (Step B), applying the coating liquid to a first transparent conductive film to obtain a coating layer (Step C), drying the coating layer to obtain a PDLC layer containing a polymer matrix and droplets containing the liquid crystal component and the dichroic dye dispersed in the polymer matrix (Step D), and laminating a second transparent conductive film on the PDLC layer (Step E).
[0053] B-1. Step A In step A, a liquid crystal component, a dichroic dye, and a dispersion medium are mixed to prepare a liquid crystal emulsion containing particles containing the liquid crystal component and the dichroic dye (hereinafter, sometimes referred to as "liquid crystal particles").
[0054] The dispersion medium is preferably water or a mixed solvent of water and a water-miscible organic solvent. Examples of the water-miscible organic solvent include C1-3 alcohol, acetone, and DMSO. The liquid crystal component and the dichroic dye are as described in Section A.
[0055] The content of the liquid crystal component in the liquid crystal emulsion is, for example, 30% to 70% by weight, and preferably 40% to 60% by weight.
[0056] The content of the dichroic dye in the liquid crystal emulsion is, for example, 0.1 to 20 parts by weight, preferably 1 to 15 parts by weight, and more preferably 3 to 10 parts by weight, per 100 parts by weight of the liquid crystal component.
[0057] The average particle size of the liquid crystal particles is typically 1 μm or less, for example, 0.5 μm or less, preferably less than 0.38 μm, more preferably less than 0.3 μm, even more preferably less than 0.2 μm, even more preferably 0.18 μm or less, even more preferably 0.15 μm or less, even more preferably 0.12 μm or less, and may be, for example, 0.01 μm or more or 0.05 μm or more. The particle size of the liquid crystal droplets in the PDLC layer may depend on the particle size of the liquid crystal particles in the liquid crystal emulsion. Therefore, as long as the average particle size of the liquid crystal particles in the liquid crystal emulsion is within the above range, the average particle size of the liquid crystal droplets in the PDLC layer can be set to the desired range. Note that the average particle size of the liquid crystal particles refers to the volume-average median diameter and can be measured using a dynamic light scattering particle size distribution analyzer.
[0058] The particle size of the liquid crystal particles preferably has a relatively narrow particle size distribution. The coefficient of variation (CV value) of the liquid crystal particles may be, for example, less than 0.4, preferably 0.35 or less, and more preferably 0.3 or less.
[0059] Liquid crystal emulsions can be prepared by, for example, mechanical emulsification, microchannel method, membrane emulsification, etc. Preferably, liquid crystal emulsions are prepared by mechanical emulsification or membrane emulsification. Mechanical emulsification can efficiently produce liquid crystal emulsions with small particle sizes. Mechanical emulsification can be performed using known dispersion / mixing devices such as homomixers and homogenizers, and is preferably performed using homogenizers such as high-pressure homogenizers and ultrasonic homogenizers. Furthermore, membrane emulsification can suitably produce emulsions with a uniform particle size distribution. For details of membrane emulsification, reference can be made to the disclosures of JP-A-4-355719 and JP-A-2015-40994 (which are incorporated herein by reference).
[0060] The order in which the liquid crystal component, the dichroic dye, and the dispersion medium are mixed is not particularly limited. For example, the liquid crystal component and the dichroic dye may be mixed together, and the resulting mixture may be mixed with the dispersion medium, or the three may be added and mixed simultaneously.
[0061] B-2. Step B In step B, the liquid crystal emulsion obtained in step A is mixed with a polymer matrix-forming resin to prepare a coating liquid containing the liquid crystal particles. The coating liquid may contain any other component as needed. Examples of the optional component include a surfactant, a leveling agent, a crosslinking agent, and a dispersion stabilizer. These optional components may be added to the liquid crystal emulsion in step A depending on the purpose.
[0062] The polymer matrix resin is as described in Section A. The polymer matrix resin is mixed with the liquid crystal emulsion, for example, as a resin dispersion in which polymer matrix resin particles are dispersed in a dispersion medium, or as a resin solution in which the polymer matrix resin is dissolved in a solvent. In this case, the dispersion medium of the resin dispersion or the solvent of the resin solution may be the same as the dispersion medium used in preparing the liquid crystal emulsion.
[0063] The average particle size of the resin particles for forming a polymer matrix is preferably 10 nm to 500 nm, more preferably 30 nm to 300 nm, and even more preferably 50 nm to 200 nm. Two or more types of resin particles differing in type and / or average particle size may be used. The average particle size of the resin particles for forming a polymer matrix means the volume-average median size and can be measured using a dynamic light scattering particle size distribution analyzer.
[0064] The particle size of the liquid crystal particles in the coating liquid is substantially the same as the particle size in the liquid crystal emulsion. Therefore, the average particle size (volume average particle size) of the liquid crystal particles in the coating liquid is typically 1 μm or less, for example, 0.5 μm or less, preferably less than 0.38 μm, more preferably less than 0.3 μm, even more preferably less than 0.2 μm, still more preferably 0.18 μm or less, still more preferably 0.15 μm or less, even more preferably 0.12 μm or less, and may be, for example, 0.01 μm or more or 0.05 μm or more.
[0065] The content of the liquid crystal component in the solid content of the coating liquid is, for example, 30 to 90% by weight, preferably 35 to 85% by weight, and more preferably 40 to 80% by weight.
[0066] The weight ratio (former:latter) of the content of the polymer matrix-forming resin to the total content of the liquid crystal component and the dichroic dye in the coating liquid is, for example, 10:90 to 70:30, preferably 15:85 to 65:35, and more preferably 20:80 to 60:40.
[0067] The total content of the polymer matrix-forming resin, the liquid crystal component, and the dichroic dye in the solid content of the coating liquid is, for example, 80% by weight or more, preferably 90% by weight or more, more preferably 95% by weight or more, and is, for example, 100% by weight or less, preferably 99% by weight or less.
[0068] Examples of the surfactant include anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, etc. The content of the surfactant is preferably 1 to 15 parts by weight, more preferably 2 to 10 parts by weight, per 100 parts by weight of the solid content of the coating liquid.
[0069] Examples of the leveling agent include an acrylic leveling agent, a fluorine-based leveling agent, a silicone-based leveling agent, etc. The content of the leveling agent is preferably 0.1 to 10 parts by weight, more preferably 0.5 to 5 parts by weight, relative to 100 parts by weight of the solid content of the coating liquid.
[0070] Examples of the crosslinking agent include an aziridine-based crosslinking agent, an isocyanate-based crosslinking agent, etc. The content of the crosslinking agent is preferably 0.5 to 20 parts by weight, more preferably 1 to 10 parts by weight, relative to 100 parts by weight of the solid content of the coating liquid.
[0071] The solid content of the coating liquid may be, for example, 20% to 60% by weight, preferably 30% to 50% by weight.
[0072] B-3. Step C In step C, the coating liquid prepared in step B is applied to the first transparent conductive film to obtain a coating layer.
[0073] The coating liquid is typically applied to the surface of the first transparent conductive film on the transparent electrode layer side. The first transparent conductive film is as described in Section A.
[0074] The viscosity of the coating liquid during application is preferably 20 mPa·s to 400 mPa·s, more preferably 30 mPa·s to 300 mPa·s, and even more preferably 40 mPa·s to 200 mPa·s. If the viscosity is less than 20 mPa·s, convection of the dispersion medium becomes significant when the dispersion medium is dried, which may result in an unstable thickness of the PDLC layer. If the viscosity exceeds 400 mPa·s, the coating liquid bead may become unstable. The viscosity of the coating liquid can be measured, for example, using an Anton Paar MCR302 rheometer. The viscosity used here is the shear viscosity value at 20°C and a shear rate of 1000 (1 / s).
[0075] Any appropriate method can be used as the coating method. For example, roll coating, spin coating, bar coating, dip coating, die coating, curtain coating, spray coating, knife coating (comma coating, etc.), etc. can be mentioned. Among them, roll coating is preferred. For example, with regard to coating by roll coating using a slot die, the description in JP-A-2019-5698 can be referred to.
[0076] The thickness of the coating layer is preferably 1 μm to 100 μm, more preferably 2 μm to 90 μm, and even more preferably 5 μm to 75 μm.
[0077] B-4. Step D In step D, the coating layer is dried to obtain a PDLC layer containing a polymer matrix and droplets containing a liquid crystal component and a dichroic dye dispersed in the polymer matrix. The dispersion medium is removed from the coating layer by drying, leaving behind the polymer matrix-forming resin and particles containing the liquid crystal component, resulting in the formation of a PDLC layer having a structure in which liquid crystal droplets are dispersed in a polymer matrix.
[0078] The coating layer can be dried by any appropriate method. Specific examples of the drying method include natural drying, heat drying, hot air drying, etc. When the coating liquid contains a crosslinking agent, a crosslinked structure of the polymer matrix can be formed during drying.
[0079] The drying temperature is preferably 20° C. to 150° C., more preferably 25° C. to 80° C. The drying time is preferably 1 minute to 100 minutes, more preferably 2 minutes to 10 minutes.
[0080] B-5. Step E In step E, a second transparent conductive film is laminated on the PDLC layer, thereby obtaining a PDLC film having the first transparent conductive film, the PDLC layer, and the second transparent conductive film in this order.
[0081] The second transparent conductive film is as described in Section A. The second transparent conductive film is typically laminated onto the PDLC layer so that the second transparent electrode layer faces the PDLC layer. From the viewpoint of obtaining sufficient adhesion, the lamination is preferably performed using a laminator while applying a lamination pressure of 0.006 MPa / m to 7 MPa / m, more preferably 0.06 MPa / m to 0.7 MPa / m.
[0082] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring each property are as follows. Unless otherwise specified, "parts" and "%" in the examples and comparative examples are by weight.
[0083] (1) Thickness: Measured using a digital micrometer (manufactured by Anritsu Corporation, product name "KC-351C"). (2) Volume average particle diameter of liquid crystal particles in liquid crystal emulsion: A measurement sample was prepared by adding a few drops of liquid crystal emulsion to 100 mL of water. Using a dynamic light scattering particle size distribution analyzer (manufactured by Microtrac, device name "Nanotrac 150"), the measurement sample was placed in the measurement holder of the device, and measurements were performed after confirming on the monitor of the device that the concentration was measurable. (3) Average particle diameter of resin particles: A measurement sample was prepared by adding a few drops of resin dispersion to 100 mL of water. Using a dynamic light scattering particle size distribution analyzer (manufactured by Microtrac, device name "Nanotrac 150"), the measurement sample was placed in the measurement holder of the device, and measurements were performed after confirming on the monitor of the device that the concentration was measurable. (4) Haze: Measured in accordance with JIS K 7136 using a haze meter (manufactured by Nippon Denshoku Industries, product name "NDH4000"). (5) Total light transmittance: Measured in accordance with JIS K 7361 using a haze meter (manufactured by Nippon Denshoku Industries, product name "NDH4000"). (6) Clarity: Measured in accordance with the manufacturer's specified method using a haze meter (manufactured by BYK-GARDNER, product name "haze-gard i"). (7) Average particle size of liquid crystal droplets in the PDLC layer: The PDLC film was sliced horizontally in a cooled environment, and the exposed horizontal cross section of the PDLC layer was smoothed using a microtome. The horizontal cross section of the PDLC layer was then observed using a scanning electron microscope (SEM), and a cross-sectional SEM image was obtained. The Heywood diameter was calculated from the cross-sectional area of all liquid crystal droplets in a 30 μm × 20 μm region in the cross-sectional SEM image, and the volume-average particle diameter (median diameter) was calculated by taking statistics weighted by the estimated volume for each equivalent diameter. (8) Birefringence of Liquid Crystal Component The value disclosed by the manufacturer of the liquid crystal component was used.
[0084] [Example 1] (First and second transparent conductive films) An ITO layer was formed on one surface of a PET substrate (thickness: 50 μm) by a sputtering method to obtain a transparent conductive film having a structure of [transparent substrate / transparent electrode layer].
[0085] (Preparation of Liquid Crystal Emulsion) A liquid crystal component containing two or more liquid crystal compounds (27.9 parts, manufactured by JNC Corporation, product name "JC-5175XX," birefringence Δn=0.09 (ne=1.569, no=1.479, dielectric anisotropy Δε=7.9, viscosity=32.2 mPa·s), 0.26 parts, dichroic dye (manufactured by Hayashibara Co., Ltd., product name "G-470"), 0.53 parts, dichroic dye (manufactured by Hayashibara Co., Ltd., product name "NKX-3739"), 1.31 parts, dichroic dye (manufactured by Hayashibara Co., Ltd., product name "NKX-3708"), 67 parts, and 3 parts of a surfactant (manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., "Noigen ET159") were mixed and treated with a high-pressure homogenizer to prepare a liquid crystal emulsion. The average particle size of the liquid crystal particles in the resulting liquid crystal emulsion was 170 nm.
[0086] (Preparation of Coating Liquid) An emulsion coating liquid (solid concentration: 30 wt %) was obtained by mixing 47.6 parts of the liquid crystal emulsion, 32 parts of an aqueous dispersion of polyether-based polyurethane resin (manufactured by DSM, product name "NeoRezR967", polymer average particle size: 80 nm, CV value = 0.27, solid content: 40 wt %), 0.1 part of a leveling agent (manufactured by DIC, product name "F-444"), 1 part of a crosslinking agent (tris[3-(2-methylaziridin-1-yl)propionic acid]=propylidinetrimethyl), and 19.3 parts of pure water.
[0087] (Production of PDLC Film) The emulsion coating liquid was applied to the ITO layer surface of the first transparent conductive film and dried at 40°C to form a PDLC layer with a thickness of 16 µm. Then, a second transparent conductive film was laminated on the PDLC layer with the ITO layer facing the PDLC layer using a laminator while applying a lamination pressure of 0.4 MPa / m. This resulted in a PDLC film.
[0088] Examples 2 to 8 PDLC films were obtained in the same manner as in Example 1, except that different types of liquid crystal components were used, liquid crystal emulsions with different average particle sizes of liquid crystal particles were prepared, and / or the thickness of the PDLC layer was changed, as shown in Table 1. The properties of the liquid crystal components used were as follows: Liquid crystal component (manufactured by JNC Corporation, product name "JC-5174XX", birefringence Δn = 0.098 (ne = 1.577, no = 1.479), dielectric anisotropy Δε = 11.8, viscosity = 46.8 mPa s) Liquid crystal component (manufactured by JNC Corporation, product name "JC-5173XX", birefringence Δn = 0.149 (ne = 1.651, no = 1.502), dielectric anisotropy Δε = 10.0, viscosity = 48.5 mPa s)
[0089] [Comparative Example 1] (First and second transparent conductive films) An ITO layer was formed on one surface of a PET substrate (thickness: 50 μm) by a sputtering method to obtain a transparent conductive film having a structure of [transparent substrate / transparent electrode layer].
[0090] (Preparation of Liquid Crystal Emulsion) 27.9 parts of a liquid crystal component (manufactured by JNC Corporation, product name "JC-5174XX"), 0.26 parts of a dichroic dye (manufactured by Hayashibara Co., Ltd., product name "G-470"), 0.53 parts of a dichroic dye (manufactured by Hayashibara Co., Ltd., product name "NKX-3739"), 1.31 parts of a dichroic dye (manufactured by Hayashibara Co., Ltd., product name "NKX-3708"), 67 parts of pure water, and 3 parts of a surfactant (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., "Noigen ET159") were mixed and roughly dispersed by stirring with a homogenizer at 100 rpm for 10 minutes. The crude dispersion was passed through a separation membrane with a uniform particle size distribution (manufactured by SPG Techno Co., Ltd., "SPG Pumping Connector", pore size 5 μm) at room temperature from the outside to the inside of the membrane at a flow rate of 80 mL / min / cm 2 This operation was repeated 10 times. The volume average particle size of the liquid crystal particles in the resulting liquid crystal emulsion was 2.1 μm.
[0091] (Preparation of Coating Liquid) An emulsion coating liquid (solid concentration: 30 wt %) was obtained by mixing 47.6 parts of the liquid crystal emulsion, 32 parts of an aqueous dispersion of polyether-based polyurethane resin (manufactured by DSM, product name "NeoRezR967", polymer average particle size: 80 nm, CV value = 0.27, solid content: 40 wt %), 0.1 part of a leveling agent (manufactured by DIC, product name "F-444"), 1 part of a crosslinking agent (tris[3-(2-methylaziridin-1-yl)propionic acid]=propylidinetrimethyl), and 19.3 parts of pure water.
[0092] (Production of PDLC Film) The emulsion coating liquid was applied to the ITO layer surface of the first transparent conductive film and dried at 40°C to form a PDLC layer with a thickness of 16 µm. Then, a second transparent conductive film was laminated on the PDLC layer with the ITO layer facing the PDLC layer using a laminator while applying a lamination pressure of 0.4 MPa / m. This resulted in a PDLC film.
[0093] Comparative Example 2 As shown in Table 1, a PDLC film was obtained in the same manner as in Comparative Example 1, except that a different type of liquid crystal component was used.
[0094] <Visual Transparency Evaluation> Visual transparency was evaluated based on the visibility of characters when plain paper on which characters were printed in black ink was visually observed through the PDLC film (colored state with no voltage applied) obtained in the Examples and Comparative Examples, according to the following criteria. The distance between the plain paper and the PDLC film was approximately 200 mm, and the distance from the observer's eye to the plain paper was 200 mm. The evaluation results, along with the clarity, total light transmittance, and haze of each PDLC film, are shown in Table 1. <Evaluation Criteria> Excellent: Transparency is very high, and characters are clearly visible. Good: Transparency is somewhat high, and characters are visible. Poor: Transparency is low, and characters are not visible.
[0095]
[0096] As shown in Table 1, the PDLC films of the examples exhibited low scattering in the colored state and high clarity.
[0097] The PDLC film of the present invention is suitable for various applications such as displays such as advertisements and guide boards, and smart windows.
[0098] 100 PDLC film 10 First transparent conductive film 20 PDLC layer 22 Polymer matrix 23 Liquid crystal component 24 Dichroic dye 25 Liquid crystal droplets 30 Second transparent conductive film
Claims
1. A polymer dispersed liquid crystal film comprising, in this order, a first transparent conductive film, a polymer dispersed liquid crystal layer, and a second transparent conductive film, wherein the polymer dispersed liquid crystal layer comprises a polymer matrix and droplets dispersed in the polymer matrix, the droplets comprising a liquid crystal component and a dichroic dye, the average particle diameter of the droplets being 1 μm or less, and the clarity in a colored state being 90 or more.
2. The polymer dispersed liquid crystal film according to claim 1, wherein the average particle size of the droplets is 0.01 μm or more and less than 0.38 μm.
3. The polymer dispersed liquid crystal film according to claim 1, wherein the birefringence of said liquid crystal component is 0.25 or less.
4. The polymer dispersed liquid crystal film according to claim 1, wherein the weight ratio (former:latter) of the content of the polymer matrix to the total content of the liquid crystal component and the dichroic dye in the polymer dispersed liquid crystal layer is 10:90 to 70:
30.
5. The polymer dispersed liquid crystal film according to claim 1, wherein the thickness of said polymer dispersed liquid crystal layer is 30 μm or less.
6. The polymer dispersed liquid crystal film according to claim 1, which has a total light transmittance of 50% or less in a colored state.
7. The polymer dispersed liquid crystal film according to claim 1, which has a haze of 80% or less in a colored state.
Citation Information
Patent Citations
Dimming sheet
JP2021196453A
Light transmittance control panel for smart windows and smart window for vehicle with the same
US20220153097A1
Dimming sheet and dimming window
WO2019132009A1
Dimming device, management method for dimming device, and production method for dimming device
WO2019221167A1