Aluminum electric wire and wire harness

The aluminum electric wire design with a central stranded wire and specific insulator characteristics addresses the flexibility and curlability issues of conventional aluminum wires, achieving improved routing and weight reduction comparable to copper wires.

WO2024203135A1PCT designated stage expired Publication Date: 2024-10-03YAZAKI CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008888
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-07
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional aluminum electric wires lack sufficient flexibility and curlability, often requiring the use of band clamps or protectors during wiring due to their tendency to bend easily, which restricts routing and interferes with equipment, unlike copper wires that are less prone to bending.

Method used

An aluminum electric wire design featuring a conductor with a central stranded wire and multiple outer layers of twisted pure aluminum strands, an insulator with a specific thickness and adhesion force range, and a crosslinked polyethylene insulator to enhance flexibility and curlability, while maintaining heat resistance and cost-effectiveness.

Benefits of technology

The improved design achieves enhanced flexibility and curlability, reducing the need for routing regulations and protectors, and offers a weight reduction comparable to copper wires while maintaining similar performance and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008888_03102024_PF_FP_ABST
    Figure JP2024008888_03102024_PF_FP_ABST
Patent Text Reader

Abstract

An aluminum electric wire (1) comprises a conductor (10) and an insulator (20). The conductor (10) is constituted by a central twisted wire (11) and a plurality of outer-circumference twisted wires (12) layered in two or more layers on the outer circumference of the central twisted wire (11). The central twisted wire (11) and the outer-circumference twisted wires (12) are formed by twisting wires formed of pure aluminum. The wires each have a wire diameter of at least 0.21 mm and less than 1.0 mm. The adhesive force between the conductor (10) and the insulator (20) is 6-45 N. The insulator (20) has a thickness of 0.72-1.80 mm.
Need to check novelty before this filing date? Find Prior Art

Description

Aluminum wires and wiring harnesses

[0001] The present invention relates to an aluminum electric wire and a wiring harness.

[0002] Conventionally, aluminum electric wires in which an insulator is coated on the outer periphery of an aluminum conductor have been proposed (see, for example, Patent Documents 1 to 3). These aluminum electric wires have improved flexibility by using a specific material for the insulator.

[0003] Japanese Patent Publication No. 2012-99412 Japanese Patent Publication No. 2012-104227 Japanese Patent Publication No. 2019-179628

[0004] However, the flexibility of an electric wire is determined by the sum of various factors, such as the material of the conductor, the diameter of the strands, the twisting configuration, the material and thickness of the insulator, and the state of adhesion between the conductor and the insulator, etc. Therefore, the electric wires described in Patent Documents 1 to 3 have room for improvement in flexibility.

[0005] Furthermore, copper electric wires are less likely to bend, resulting in a larger bending radius during installation. For this reason, protectors or band clamps have been used to restrict the length of copper electric wires to prevent interference with other equipment and electric wires. In contrast, aluminum electric wires are more likely to bend than copper electric wires. However, even aluminum electric wires still lack sufficient bending properties, and some require the use of band clamps or other methods to restrict the length of wires.

[0006] The present invention has been made to solve the above-mentioned problems in the prior art, and one of the objects of the invention is to provide an aluminum electric wire and a wiring harness that can achieve improved flexibility and shapeability.

[0007] An aluminum electric wire according to one embodiment of the present invention includes a conductor and an insulator covering the conductor, the conductor being composed of a central strand and a plurality of peripheral strands laminated in two or more layers around the central strand, the central strand and the peripheral strand being constructed by twisting together strands of pure aluminum, and the strands each having a diameter of 0.21 mm or more and less than 1.0 mm, an adhesion strength between the conductor and the insulator being 6 N or more and 45 N or less, and the insulator having a thickness of 0.72 mm or more and 1.80 mm or less.

[0008] A wire harness according to one embodiment of the present invention includes the aluminum electric wire described above.

[0009] According to the present invention, it is possible to provide an aluminum electric wire and a wiring harness that can be improved in flexibility and shapeability.

[0010] FIG. 1 is a perspective view showing an example of a wire harness including an aluminum electric wire according to an embodiment of the present invention. FIG. 2 is a cross-sectional view showing an example of the aluminum electric wire shown in FIG. 1. FIG. 3 is a cross-sectional view showing an example of a partial configuration of the aluminum electric wire shown in FIG. 2. FIG. 4 is a first diagram showing examples and comparative examples. FIG. 5 is a second diagram showing examples and comparative examples. FIG. 6A is a schematic diagram showing a method for measuring adhesion, illustrating a sample for measuring adhesion. FIG. 6B is a schematic diagram showing a method for measuring adhesion, illustrating the method for measuring adhesion. FIG. 7 is a conceptual diagram showing the state of a flexibility test. FIG. 8 is a diagram showing the results of a curling property test. FIG. 9 is a diagram showing the results of a comparison between the aluminum electric wire of Example 3 and the copper electric wire of Comparative Example 10.

[0011] The present invention will be described below in accordance with a preferred embodiment. Note that the present invention is not limited to the embodiment described below and can be modified as appropriate without departing from the spirit of the present invention. In addition, in the embodiment described below, some components are omitted from illustration and description, but it goes without saying that publicly known or well-known technologies are applied as appropriate to the details of the omitted technologies within the scope of the content described below.

[0012] Fig. 1 is a perspective view showing an example of a wire harness including an aluminum electric wire according to an embodiment of the present invention. As shown in Fig. 1, the wire harness WH is configured to include an aluminum electric wire 1 and other members O. The other members O are, for example, connectors O1 and terminals O2. Note that the other members O are not limited to the connectors O1 and terminals O2, and may be other electric wires, etc.

[0013] Fig. 2 is a cross-sectional view showing an example of the aluminum electric wire 1 shown in Fig. 1, and Fig. 3 is a cross-sectional view showing an example of a partial configuration of the aluminum electric wire 1 shown in Fig. 2. As shown in Fig. 2, the aluminum electric wire 1 includes a conductor 10 and an insulator 20 that covers the outer periphery of the conductor 10 in contact with each other.

[0014] The conductor 10 includes a central stranded wire 11 and a plurality of peripheral stranded wires 12. The plurality of peripheral stranded wires 12 are arranged to form two or more layers around the central stranded wire 11. The peripheral stranded wires 12 are assumed to be bunch-twisted around the central stranded wire 11, but are not limited to bunch-twisting and may be concentrically twisted. As shown in FIG. 3, the central stranded wire 11 and the peripheral stranded wire 12 are formed by twisting a plurality of wires 11a, 12a made of pure aluminum.

[0015] In this embodiment, the wires 11a, 12a constituting the central stranded wire 11 and the peripheral stranded wire 12 have a diameter of 0.21 mm or more and less than 1.0 mm. If the wire diameter is less than 0.21 mm, the wires 11a, 12a are too thin and prone to breakage, whereas if the wire diameter is 1.0 mm or more, the wires 11a, 12a are too thick and lose flexibility.

[0016] In this embodiment, the adhesive force between the conductor 10 and the insulator 20 is 6 N or more and 45 N or less. If the adhesive force is less than 6 N, the conductor 10 and the insulator 20 will move too easily independently when bending the wire, significantly reducing the ability to form the wire. If the adhesive force exceeds 45 N, the adhesive force will be too strong, making it difficult for the conductor 10 and the insulator 20 to move independently, causing them to act like a thick rod and reducing flexibility.

[0017] Furthermore, in this embodiment, the thickness of the insulator 20 is 0.72 mm or more and 1.80 mm or less. If the thickness is less than 0.72 mm, the insulator 20 is too thin to ensure wear resistance. If the thickness exceeds 1.80 mm, the insulator 20 is too thick to ensure flexibility.

[0018] Additionally, in this embodiment, the insulator 20 is preferably made of cross-linked polyethylene, because cross-linked polyethylene strikes a balance between heat resistance and cost, making it easier to provide an aluminum electric wire 1 that is more excellent in heat resistance and cost.

[0019] The cross-sectional area (size) of the conductor 10 is preferably 30 sq. or more and 230 sq. or less. If the cross-sectional area is less than 30 sq., the weight reduction effect is reduced compared to a copper electric wire of the same size. If the cross-sectional area exceeds 230 sq., the size becomes too large, making it difficult to apply to, for example, a vehicle.

[0020] Furthermore, it is preferable that the twist pitch of the central stranded wire 11 is 15 to 30 times (preferably 20 times) the twist outer diameter, and that the twist pitch of the peripheral stranded wires 12 is 8 to 15 times (preferably 11 times) the outer diameter of the corresponding layer. Here, the corresponding layer refers to the first layer in the case of the peripheral stranded wires 12 belonging to the first layer, and the second layer in the case of the peripheral stranded wires 12 belonging to the second layer. That is, it is preferable that the twist pitch of the peripheral stranded wires 12 in the first layer is 8 to 15 times (preferably 8 to 15 times) the outer diameter of the first layer, and the twist pitch of the peripheral stranded wires 12 in the second layer is 8 to 15 times (preferably 8 to 15 times) the outer diameter of the second layer. Adopting these twist pitches can contribute to preventing wire breakage, loose twist, and twist collapse.

[0021] Next, examples of the present invention and comparative examples will be described. Figures 4 and 5 are diagrams showing examples and comparative examples.

[0022] First, as shown in Figures 4 and 5, all of the wires constituting the conductor in Example 1 were made of pure aluminum. The conductor size in Example 1 was 50 sq. m, and the central strand and the outer strand had 19 strands in the main twist and 32 strands in the undertwist, with a wire diameter of 0.32 mm. The cross-sectional area of ​​such a conductor was 48.9 mm. 2 The outer diameter was 10.0 mm. In Example 1, the insulator was made of cross-linked polyethylene (PE) with a thickness of 1.50 mm. The aluminum electric wire according to Example 1 had an outer diameter of 13.0 mm. Furthermore, the adhesion force was measured using a measurement method in accordance with ISO 19642, which will be described later, and the adhesion force was found to be 6 N.

[0023] The aluminum electric wire according to Example 2 was the same as that of Example 1 except that the adhesive force was 45N.

[0024] In Example 3, all the wires were made of pure aluminum. The conductor size was 95 sq., and the central strand and the outer strand had 19 strands in the main twist and 62 strands in the under twist, with a wire diameter of 0.32 mm. The cross-sectional area of ​​such a conductor was 94.7 mm. 2 The outer diameter was 13.9 mm. In Example 3, the insulator was made of cross-linked polyethylene and had a thickness of 1.50 mm. The aluminum electric wire according to Example 3 had an outer diameter of 16.9 mm. Furthermore, the adhesion force was 9 N.

[0025] On the other hand, in Comparative Example 1, all of the wires constituting the conductor were made of pure copper. Also, in Comparative Example 1, the conductor size was 30 sq., and the central strand and the outer strand had 19 strands in the main twist and the under twist, and the wire diameter was 0.32 mm. The cross-sectional area of ​​such a conductor was 29.0 mm. 2 The outer diameter was 7.8 mm. In Comparative Example 1, the insulator was made of cross-linked polyethylene and had a thickness of 1.30 mm. The aluminum electric wire according to Comparative Example 1 had an outer diameter of 10.4 mm. Furthermore, the adhesion force was 86 N.

[0026] In Comparative Example 2, all of the wires constituting the conductor were made of pure copper. The conductor size was 35 sq. m, and the central strand and the outer strand had 19 strands in the main twist and 23 strands in the under twist, with a wire diameter of 0.32 mm. The cross-sectional area of ​​such a conductor was 35.2 mm. 2 The outer diameter was 8.4 mm. In Comparative Example 2, the insulator was made of cross-linked polyethylene and had a thickness of 1.50 mm. The aluminum electric wire according to Comparative Example 2 had an outer diameter of 11.4 mm. Furthermore, the adhesion force was 95 N.

[0027] In Comparative Example 3, all of the wires constituting the conductor were made of pure copper. The conductor size was 40 sq. m, and the central strand and the outer strand had 19 strands in the main twist and 26 strands in the under twist, with a wire diameter of 0.32 mm. The cross-sectional area of ​​such a conductor was 39.7 mm. 2 The outer diameter was 9.1 mm. In Comparative Example 3, the insulator was made of cross-linked polyethylene and had a thickness of 1.40 mm. The electric wire according to Comparative Example 3 had an outer diameter of 11.9 mm. Furthermore, the adhesion force was 110 N.

[0028] In Comparative Example 4, all of the wires constituting the conductor were made of pure aluminum. The conductor size was 50 sq. m, and the central strand and the outer strand had 19 strands in the main twist and 83 strands in the under twist, with a wire diameter of 0.20 mm. The cross-sectional area of ​​such a conductor was 50.6 mm. 2 The outer diameter was 9.9 mm. In Comparative Example 4, the insulator was made of cross-linked polyethylene and had a thickness of 1.50 mm. The aluminum electric wire according to Comparative Example 4 had an outer diameter of 12.9 mm. This aluminum electric wire had wire breakage during production and was therefore not suitable for use as a product, so measurements of adhesion and the like were not performed.

[0029] In Comparative Example 5, all of the wires constituting the conductor were made of pure aluminum. The conductor size was 50 sq. m, and the central strand and the outer strand had 19 strands in the main twist and 32 strands in the under twist, with a wire diameter of 0.32 mm. The cross-sectional area of ​​such a conductor was 48.9 mm. 2The outer diameter was 10.0 mm. In Comparative Example 5, the insulator was made of cross-linked polyethylene and had a thickness of 0.50 mm. The aluminum electric wire according to Comparative Example 5 had an outer diameter of 11.0 mm. Note that this aluminum electric wire was not viable as a product because the thickness of the insulator was too thin to ensure wear resistance and the coating thickness was unstable. For this reason, measurements of adhesion and the like were not performed on Comparative Example 5.

[0030] In Comparative Example 6, the conductor was the same as in Comparative Example 5. In addition, in Comparative Example 6, the insulator was made of cross-linked polyethylene and had a thickness of 0.72 mm. The aluminum electric wire according to Comparative Example 6 had an outer diameter of 11.4 mm. The adhesion force was 5 N.

[0031] In Comparative Example 7, the conductor was the same as in Comparative Example 5. In addition, in Comparative Example 7, the insulator was made of cross-linked polyethylene and had a thickness of 1.80 mm. The aluminum electric wire according to Comparative Example 7 had an outer diameter of 13.6 mm. The adhesion force was 52 N.

[0032] In Comparative Example 8, all of the wires constituting the conductor were made of pure aluminum. The conductor size in Comparative Example 8 was 50 sq. m, and the stranded wire was made by twisting 61 wires each having a wire diameter of 1.0 mm. The cross-sectional area of ​​such a conductor was 47.9 mm. 2 The outer diameter was 9.0 mm. In Comparative Example 8, the insulator was made of cross-linked polyethylene and had a thickness of 1.50 mm. The aluminum electric wire according to Comparative Example 8 had an outer diameter of 12.0 mm. Furthermore, the adhesion force was 28 N.

[0033] In Comparative Example 9, all of the wires constituting the conductor were made of pure aluminum. The conductor size was 50 sq. m, and the central strand and the outer strand had 19 main strands and 13 under-twisted strands, with a wire diameter of 0.5 mm. The cross-sectional area of ​​such a conductor was 48.5 mm. 2 The outer diameter was 9.4 mm. In Comparative Example 9, the insulator was made of cross-linked polyethylene and had a thickness of 1.50 mm. The aluminum electric wire according to Comparative Example 9 had an outer diameter of 12.4 mm. Furthermore, the adhesion force was 200 N.

[0034] In Comparative Example 10, all of the wires constituting the conductor were made of pure copper. The conductor size was 70 sq. m, and the central strand and the outer strand had 19 strands in the main twist and 46 strands in the under twist, with a wire diameter of 0.32 mm. The cross-sectional area of ​​such a conductor was 70.3 mm. 2 The outer diameter was 12.0 mm. In Comparative Example 10, the insulator was made of cross-linked polyethylene and had a thickness of 1.50 mm. The electric wire according to Comparative Example 10 had an outer diameter of 15.0 mm. Furthermore, the adhesion force was 120 N.

[0035] In Comparative Example 11, all of the wires constituting the conductor were made of pure aluminum. The conductor size was 95 sq. m, and the central strand and the outer strand had 19 strands in the main twist and 25 strands in the under twist, with a wire diameter of 0.5 mm. The cross-sectional area of ​​such a conductor was 93.2 mm. 2 The outer diameter was 12.9 mm. In Comparative Example 11, the insulator was made of cross-linked polyethylene and had a thickness of 1.50 mm. The aluminum electric wire according to Comparative Example 11 had an outer diameter of 15.9 mm. Furthermore, the adhesion force was 55 N.

[0036] In Comparative Example 12, all of the wires constituting the conductor were made of aluminum alloy. The conductor size was 50 sq., and the central strand and the outer strand had 19 strands in the main twist and 32 strands in the under twist, with a wire diameter of 0.32 mm. The cross-sectional area of ​​such a conductor was 48.9 mm. 2 The outer diameter was 10.0 mm. In Comparative Example 12, the insulator was made of cross-linked polyethylene and had a thickness of 1.50 mm. The aluminum electric wire according to Comparative Example 12 had an outer diameter of 13.0 mm. Furthermore, the adhesion force was 54 N.

[0037] The adhesion was measured as follows: Fig. 6A is a schematic diagram showing the adhesion measurement method, illustrating a sample for measuring the adhesion. Fig. 6B is a schematic diagram showing the adhesion measurement method, illustrating the adhesion measurement method.

[0038] To measure the adhesion, first, a 25 mm length of insulation was stripped off from one end of a 75 mm long electric wire to expose the conductor, as shown in Fig. 6A. Then, as shown in Fig. 6B, the conductor was inserted into a hole in a plate having a diameter 0.1 mm larger than the outer diameter of the conductor, and the conductor was pulled from the insertion side at a speed of 200 mm / min until the conductor was separated from the insulation, and the force (maximum) when the conductor was pulled out was taken as the adhesion.

[0039] The electric wires of Examples 1 to 3 and Comparative Examples 1 to 12 were subjected to a flexibility test, and the electric wires of Examples 1 to 3 and Comparative Examples 2 and 6 were subjected to a curling test.

[0040] Fig. 7 is a conceptual diagram showing the flexibility test. For the flexibility test, a 400 mm electric wire with an insulator coated on a conductor was used as a sample. As shown in Fig. 7, the other end of the sample was fixed, and a load was applied from one end. The load at which the sample was bent 180 degrees was taken as the flexibility.

[0041] Fig. 8 is a table showing the results of the formability test. In the formability test, as shown in Fig. 8, electric wires were wound around cylinders of φ75 and φ50, secured with cable ties or the like, left to stand for one minute, and then released, and the extent to which the electric wires spread was evaluated. Regarding the evaluation in Figs. 4 and 5, if the spread of the electric wire on a line passing through the center of the cylinder (see the dashed line in Fig. 8) was 75 mm or more, the formability was evaluated as "x", and if it was less than 75 mm, the formability was evaluated as "o". The reason for using cylinders of φ75 and φ50 is to check the formability of the electric wire at approximately five times the diameter.

[0042] As shown in Figures 4 and 5, Examples 1 to 3 had flexibility of 7N or more and 11N or less, resulting in excellent flexibility. Similarly, Comparative Examples 1, 2, and 6 also had excellent flexibility. In particular, it was found that the aluminum electric wires of Examples 1 to 3 were thicker than the copper electric wires of Comparative Examples 1 and 2, but were able to exhibit the same degree of flexibility. On the other hand, Comparative Examples 3 and 7 to 12 had flexibility exceeding 11N, and did not achieve the same level of flexibility as Examples 1 to 3. Note that Comparative Examples 4 and 5 were not viable as products, and flexibility measurements were not performed.

[0043] 4, 5, and 8, in Examples 1 to 3 (Example 3 is omitted in Fig. 8), the spread of the aluminum electric wire was less than 75 mm, and the shapeability was good, that is, the electric wire did not require route restriction by a protector or band clamp. On the other hand, in Comparative Examples 2 and 6 (Comparative Example 2 is omitted in Fig. 8), the spread of the electric wire was 75 mm or more, and route restriction was required.

[0044] From the above, it was found that the aluminum electric wires according to Examples 1 to 3 were able to improve flexibility and shapeability.

[0045] The aluminum electric wires according to the examples do not have a significantly larger outer diameter than copper electric wires, and therefore can be significantly lighter. Fig. 9 is a table showing the results of a comparison between the aluminum electric wire of Example 3 and the copper electric wire of Comparative Example 10. When the ambient temperature was 105°C and a current of 250 A was continuously applied, as shown in Fig. 9, the maximum temperature of the conductor of the aluminum electric wire according to Example 3 was 136.9°C, and the maximum temperature of the conductor of the copper electric wire according to Comparative Example 10 was 137.2°C. In other words, the two had approximately the same temperature.

[0046] Comparing the outer diameters of the electric wires, the aluminum electric wire according to Example 3 was 16.9 mm, and the copper electric wire according to Comparative Example 10 was 15.0 mm. That is, the aluminum electric wire according to Example 3 had an outer diameter of about 113.5% of that of the copper electric wire according to Comparative Example 10, and there was not a large difference between the two.

[0047] In contrast, when comparing the weights, the aluminum electric wire according to Example 3 had a weight of 288.5 g / m, while the copper electric wire according to Comparative Example 10 had a weight of 731.3 g / m. That is, the aluminum electric wire according to Example 3 had a weight that was reduced by approximately 60.6% compared to the copper electric wire according to Comparative Example 10.

[0048] Thus, in the aluminum electric wire 1 and the wire harness WH according to this embodiment, the conductor 10 is not only composed of the central stranded wire 11 and the outer circumferential stranded wire 12 formed by twisting the element wires 11 a, 12 a, but also has a wire diameter of less than 1.0 mm. This prevents the element wires 11 a, 12 a from becoming too thick and impairing the flexibility of the aluminum electric wire 1. Furthermore, since the element wire diameter is 0.21 mm or more, the possibility of the electric wire breaking when being bent is reduced.

[0049] Furthermore, since the adhesive force between the conductor 10 and the insulator 20 is 6 N or more, a certain degree of adhesive force is ensured, making it difficult for the conductor 10 and the insulator 20 to move separately, and reducing the deterioration of the formability that would otherwise occur if each of them moved independently. Also, since the adhesive force between the conductor 10 and the insulator 20 is 45 N or less, the conductor 10 and the insulator 20 are integrated, reducing the reduction in flexibility that would occur when bending a thick object.

[0050] In addition, since the thickness of the insulator 20 is 0.72 mm or more and 1.80 mm or less, the insulator 20 is prevented from being too thin to ensure wear resistance, or from being too thick to reduce flexibility.

[0051] Therefore, it is possible to provide an aluminum electric wire 1 and a wire harness WH that can achieve improved flexibility and shapeability.

[0052] Furthermore, since the insulator 20 is made of cross-linked polyethylene, it is possible to provide an aluminum electric wire 1 that is superior in both heat resistance and cost by achieving a good balance between both.

[0053] Furthermore, since the conductor 10 has a cross-sectional area of ​​30 sq. or more, it has a certain degree of weight reduction effect compared to copper wires of the same size, while the cross-sectional area is 230 sq. or less, so it does not become too large and can be easily applied to vehicles, for example.

[0054] The twist pitch of the central stranded wire 11 is 15 to 30 times the twist outer diameter, and the twist pitch of the peripheral stranded wire 12 is 8 to 15 times the twist outer diameter, which greatly reduces the possibility of exceeding the processing limit and helps prevent wire breakage, loose twist, and loose twist.

[0055] The present invention has been described above based on one embodiment, but the present invention is not limited to the above embodiment, and modifications may be made or well-known and well-known technologies may be combined within the scope of the invention.

[0056] For example, in the wire harness WH according to the present embodiment, the connectors O1 and the terminals O2 are exemplified as examples of the other members O, but the other members O are not particularly limited to these and may be, for example, the same type of aluminum electric wire 1 or the like.

[0057] Here, the features of one embodiment of the present invention are briefly summarized below: [1] An aluminum electric wire (1) comprising a conductor (10) and an insulator (20) covering the conductor (10), the conductor (10) being composed of a central strand (11) and a plurality of peripheral strands (12) stacked in two or more layers around the central strand (11), the central strand (11) and the peripheral strand (12) being composed of strands of wires (11a, 12a) made of pure aluminum, wherein the wires (11a, 12a) each have a diameter of 0.21 mm or more and less than 1.0 mm, the adhesion between the conductor (10) and the insulator (20) is 6 N or more and 45 N or less, and the insulator (20) has a thickness of 0.72 mm or more and 1.80 mm or less. [2] The aluminum electric wire (1) according to the above [1], wherein the insulator (20) is cross-linked polyethylene. [3] The aluminum electric wire (1) according to the above [1], wherein the conductor (10) has a cross-sectional area of ​​30 sq or more and 230 sq or less. [4] The aluminum electric wire (1) according to the above [1], wherein, in the conductor (10), the twist pitch of the central stranded wire (11) is 15 to 30 times the twist outer diameter, and the twist pitch of the peripheral stranded wire (12) is 8 to 15 times the outer diameter of the corresponding layer. [5] A wire harness (WH) comprising the aluminum electric wire (1) according to any one of the above [1] to [4].

[0058] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the invention.

[0059] This application is based on a Japanese patent application (Patent Application No. 2023-57192) filed on March 31, 2023, the contents of which are incorporated herein by reference.

[0060] According to the present invention, it is possible to provide an aluminum electric wire and a wiring harness that can be improved in flexibility and shapeability. The present invention that exhibits this effect is useful for aluminum electric wires and wiring harnesses.

[0061] 1: Aluminum electric wire 10: Conductor 11: Central stranded wire 12: Peripheral stranded wire 11a, 12a: Wires 20: Insulator O: Other member WH: Wire harness

Claims

1. An aluminum electric wire comprising a conductor and an insulator covering the conductor, the conductor being composed of a central strand and a plurality of peripheral strands stacked in two or more layers around the central strand, the central strand and the peripheral strand being composed of strands of pure aluminum, wherein the diameter of each of the strands is 0.21 mm or more and less than 1.0 mm, the adhesion between the conductor and the insulator is 6 N or more and 45 N or less, and the thickness of the insulator is 0.72 mm or more and 1.80 mm or less.

2. The aluminum electric wire according to claim 1, wherein the insulation is cross-linked polyethylene.

3. An aluminum electric wire according to claim 1, wherein the conductor has a cross-sectional area of ​​30 sq. or more and 230 sq. or less.

4. An aluminum electric wire according to claim 1, wherein the conductor has a twist pitch of the central stranded wire that is 15 to 30 times the twist outer diameter, and a twist pitch of the peripheral stranded wire that is 8 to 15 times the outer diameter of the corresponding layer.

5. A wire harness comprising the aluminum electric wire according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Resin composition and electric wire for automobile covered with the resin composition

    JP2012229343A

  • Bending-resistant electric wire and wiring harness

    JP2016197569A

  • Highly flexible insulated wire

    JP2019021560A

  • Insulation wire

    JP2019207811A