Method for manufacturing laminate
The method addresses the low elastic modulus issue in conventional curable resin compositions by using a specific epoxy resin and dicyandiamide composition, ensuring high elastic modulus in both room and high-temperature conditions, suitable for automotive structural adhesives with reduced curing time and energy consumption.
Patent Information
- Application Number
- PCT/JP2024/008925
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-08
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional curable resin compositions used in bonding adherends have a low elastic modulus at high temperatures when cured at low temperatures and in short times, leading to inadequate performance in high-temperature environments, particularly in automotive applications where structural adhesives require high mechanical strength and durability.
A method for manufacturing a laminate using a specific curable resin composition comprising unmodified bisphenol A type epoxy resin and dicyandiamide, cured at temperatures between 105°C to 145°C for 10 to 60 minutes, which maintains a high elastic modulus in high-temperature environments by controlling the thickness ratio of the cured product to the adherends and optimizing the composition with polymer particles and curing agents.
The method ensures a laminate with a high elastic modulus in both room and high-temperature conditions, enhancing the durability and mechanical strength of bonded adherends, particularly suitable for automotive structural adhesives, while reducing curing time and energy consumption.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Manufacturing method of laminate
[0001] The present invention relates to a method for producing a laminate.
[0002] Curable resin compositions containing epoxy resins are excellent in many respects, such as dimensional stability, mechanical strength, electrical insulation properties, heat resistance, water resistance, and chemical resistance, and are used in a variety of applications.
[0003] One known application of such a curable resin composition containing an epoxy resin is as a structural adhesive for automobiles. Patent Documents 1 and 2 disclose techniques relating to a curable resin composition containing an epoxy resin.
[0004] Japanese Patent Publication No. 2019-038926 International Publication No. WO2018 / 156450
[0005] However, conventional curable resin compositions such as those described in Patent Documents 1 and 2 have had a problem in that when the curable resin composition is used to bond adherends and cured at a low temperature for a short time, the modulus of elasticity of the cured product in the resulting laminate, particularly the modulus of elasticity at high temperatures, is significantly reduced.
[0006] In view of the current situation as described above, an object of the present invention is to provide a laminate in which adherends are bonded to each other by a cured product that has a high elastic modulus in a high-temperature environment even when cured at a low temperature for a short time.
[0007] The present inventors have conducted extensive research to solve the above problems and have completed the present invention.
[0008] That is, one embodiment of the present invention is a method for producing a laminate in which a first adherend, a cured product obtained by curing a curable resin composition, and a second adherend are laminated in this order, the method comprising: a step (i) of applying the curable resin composition to the first adherend and laminating the second adherend to the first adherend (laminating step); and a step (ii) of curing the curable resin composition (curing step), wherein the curable resin composition is a mixture of an epoxy resin (A) and 3.5 parts by mass of dicyandiamide (B) per 100 parts by mass of the epoxy resin (A). the epoxy resin (A) contains 51% by mass to 100% by mass of an unmodified bisphenol A epoxy resin (A-1) relative to a total amount (100% by mass) of the epoxy resin (A); the curing temperature of the curable resin composition in the step (ii) is 105°C to 145°C; the curing time of the curable resin composition in the step (ii) is 10 minutes to 60 minutes; and the ratio (Y / X) of the thickness (Y) of the cured product to the average thickness (X) of the first adherend and the second adherend is 0.5 to 10.0.
[0009] According to one embodiment of the present invention, it is possible to provide a laminate in which an adherend is bonded to a cured product that has a high elastic modulus in a high-temperature environment, even when cured at a low temperature for a short time.
[0010] One embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to the respective configurations described below, and various modifications are possible within the scope of the claims. Embodiments and examples obtained by appropriately combining the technical means disclosed in different embodiments and examples are also included in the technical scope of the present invention. Furthermore, all academic literature and patent documents described in this specification are incorporated herein by reference. Furthermore, unless otherwise specified in this specification, "A to B" representing a numerical range means "greater than or equal to A and less than or equal to B."
[0011] [1. Technical Concept of the Present Invention] In response to the recent trend toward carbon neutrality, there is a need to lower the temperature of the baking oven for electrodeposition coating (anti-rust primer paint for automobiles), and the baking temperature during electrodeposition coating, which was previously 170 to 190° C., has been lowered to approximately 120 to 145° C. There is also a demand for a shorter baking time (within 60 minutes).
[0012] During the automobile manufacturing process, automotive structural adhesives are usually cured simultaneously with electrodeposition paint in the above-mentioned baking oven. For this reason, structural adhesives are also required to cure at low temperatures (145°C or less) and in a short time.
[0013] Furthermore, automotive structural adhesives are required to have a high modulus of elasticity not only under normal conditions (for example, at room temperature) but also under high-temperature conditions such as in summer.
[0014] However, it has been found that conventional curable resin compositions such as those described in Patent Documents 1 and 2 have a problem in that when the curable resin composition is cured at a low temperature for a short time, the resulting cured product has a low Tg. As a result, it has also been found that a cured product obtained by bonding an adherend using the curable resin composition and a laminate including the cured product have a problem in that the modulus of elasticity is low in a high-temperature environment.
[0015] In light of the above-mentioned circumstances, the present inventors have conducted extensive research with the aim of providing a laminate in which adherends are bonded to a cured product that has a high elastic modulus in a high-temperature environment even when cured at a low temperature for a short time. Through their research, the present inventors have made the novel discovery that, when a specific curable resin composition is cured at a low temperature for a short time, there is a correlation between the ratio (Y / X) of the thickness (Y) of the cured product obtained by curing the curable resin composition to the average thickness (X) of the adherends adhered to the cured product, and the glass transition temperature (hereinafter sometimes referred to as "Tg") of the cured product. As a result of further intensive research based on this new finding, the present inventors have discovered that by (1) using a curable resin composition having a specific composition, and (2) controlling the ratio (Y / X) of the thickness (Y) of the cured product obtained by curing the curable resin composition to the average thickness (X) of the adherends adhered by the cured product within a specific range, it is possible to provide a laminate in which adherends are bonded to a cured product having a high elastic modulus in a high-temperature environment, even when the curing is performed at a low temperature for a short time, and have completed the present invention.
[0016] The technology for bonding (laminating) adherends with a cured product that has a high elastic modulus in a high-temperature environment even when cured at a low temperature for a short time is not known in the past, and can be said to be a surprising discovery. Furthermore, this method for producing a laminate is extremely useful, particularly in the production of automobile body structures.
[0017] [2. Method for manufacturing a laminate] A method for manufacturing a laminate according to one embodiment of the present invention is a method for manufacturing a laminate in which a first adherend, a cured product obtained by curing a curable resin composition, and a second adherend are laminated in this order, the method comprising: a step (i) of applying the curable resin composition to the first adherend and laminating the second adherend to the first adherend (laminating step); and a step (ii) of curing the curable resin composition (curing step), wherein the curable resin composition is a mixture of an epoxy resin (A) and dicyandiamine, and the curable resin composition is a curable resin composition containing 100 parts by mass of the epoxy resin (A) and 100 parts by mass of the epoxy resin (A). The epoxy resin (A) contains 51% by mass to 100% by mass of an unmodified bisphenol A epoxy resin (A-1), the curing temperature of the curable resin composition in step (ii) is 105°C to 145°C, the curing time of the curable resin composition in step (ii) is 10 minutes to 60 minutes, and the ratio (Y / X) of the thickness (Y) of the cured product obtained by curing the curable resin composition to the average thickness (X) of the first adherend and the second adherend is 0.5 to 10.0. Hereinafter, the "method for producing a laminate according to one embodiment of the present invention" may be referred to as "the present production method," "epoxy resin (A)" may be referred to as "component (A)," and "dicyandiamide (B)" may be referred to as "component (B)."
[0018] According to this production method, even when cured at low temperature for a short time, it is possible to provide a laminate in which adherends are bonded by a cured product that has a high elastic modulus in a high-temperature environment.
[0019] (2-1. Curable Resin Composition) The curable resin composition used in the present production method will be described in detail below. A curable resin composition according to one embodiment of the present invention (hereinafter, may be referred to as the "present curable resin composition") contains 3.5 to 19.0 parts by mass of component (B) per 100 parts by mass of component (A). A cured product can be obtained by curing the present curable resin composition by the method described in the curing step below.
[0020] Each component that may be contained in the curable resin composition will be described in detail below.
[0021] <Epoxy Resin (A)> In this specification, the term "epoxy resin" refers to a resin having at least one epoxy group, preferably two or more epoxy groups, in the molecule. Examples of epoxy resins that the present curable resin composition may contain as component (A) include unmodified bisphenol A-type epoxy resin (A-1) (hereinafter sometimes referred to as "component (A-1)"), unmodified bisphenol F-type epoxy resin (A-2) (hereinafter sometimes referred to as "component (A-2)"), aliphatic polybasic acid-modified epoxy resin (A-3) (hereinafter sometimes referred to as "component (A-3)"), and other epoxy resins (other than components (A-1) to (A-3)). In this specification, component (A) refers collectively to these epoxy resins contained in the present curable resin composition. For example, in this specification, the amount of component (A) refers to the total amount of components (A-1), (A-2), (A-3), and other epoxy resins contained in the present curable resin composition. Component (A) can also be said to be a curable resin.
[0022] The content of component (A) in the present curable resin composition is not particularly limited, but is preferably 20% by mass to 80% by mass, more preferably 25% by mass to 75% by mass, and even more preferably 35% by mass to 55% by mass, relative to 100% by mass of the total amount of the present curable resin composition. If the content of component (A) in the present curable resin composition is 20% by mass or more, there is an advantage that the strength and adhesive strength of the obtained cured product are excellent, and if it is 80% by mass or less, there is an advantage that the workability of the curable resin composition is excellent.
[0023] (Unmodified Bisphenol A Epoxy Resin (A-1)) Component (A) contains 51% to 100% by mass of component (A) in a total amount of 100% by mass. The content of component (A-1) in component (A) is 51% to 100% by mass, preferably 55% to 90% by mass, and more preferably 60% to 80% by mass, in a total amount of 100% by mass of component (A). When the content of component (A-1) in component (A) contained in the curable resin composition is within the above range, a cured product having an excellent elastic modulus in a high-temperature environment can be provided. The epoxy equivalent of component (A-1) is not particularly limited, but is preferably 150 to 1,000, more preferably 160 to 500, and even more preferably 170 to 200. When the epoxy equivalent of component (A-1) is 150 or more, the adhesive strength and high-temperature rigidity of the resulting cured product tend to be improved, and when it is 1000 or less, the handleability of the curable resin composition tends to be improved.
[0024] In this specification, the term "epoxy equivalent" refers to the molecular weight per epoxy group contained in a compound having an epoxy group, and specifically, is a value calculated based on the following formula: Epoxy equivalent (g / eq) = mass average molecular weight (Mw) of compound / number of epoxy groups per molecule of compound (average number). The epoxy equivalent can also be measured in accordance with JIS K7236.
[0025] Examples of commercially available component (A-1) include those commercially available under the trade name jER from Mitsubishi Chemical Corporation (e.g., jER828, jER825, jER827, jER828EL, jER828US, jER828XA, jER834, jER1001, jER1002, jER1004, jER1007, jER1009, jER1010), and those commercially available under the trade name jER from Momentive Specialty Chemicals, Inc. those commercially available under the trade name EPON from Olin Epoxy Co. (e.g., EPON 1510, EPON 1310, EPON 828, EPON 872, EPON 1001, EPON 1004, EPON 2004); Examples of suitable resins include, but are not limited to, resins commercially available under the trade name DER from Epson Corporation (e.g., DER 331, DER 332, DER 336, and DER 439), resins commercially available under the trade name ADEKA RESIN from ADEKA Corporation (e.g., EP-4100, EP-4300, EP-4400, EP-4530, and EP-4504), and resins commercially available under the trade name EPICLON from DIC Corporation (e.g., EPICLON 840 and EPICLON 850).
[0026] (Unmodified Bisphenol F Epoxy Resin (A-2)) Component (A) may contain component (A-2) in addition to component (A-1). When the curable resin composition contains component (A-2) as component (A), the content of component (A-2) in component (A) is preferably 1% by mass to 80% by mass, more preferably 5% by mass to 50% by mass, and even more preferably 10% by mass to 30% by mass, relative to the total amount of component (A) (100% by mass). When component (A) contained in the curable resin composition contains component (A-2) in the above range, it is possible to provide a curable resin composition that has low viscosity and excellent workability, and that produces a cured product with excellent toughness and adhesive strength.
[0027] The epoxy equivalent of component (A-2) is not particularly limited, but is preferably 150 to 1,000, more preferably 160 to 500, and even more preferably 170 to 200. When the epoxy equivalent of component (A-2) is 150 or more, there is an advantage that the resulting cured product has excellent adhesive strength and rigidity at high temperatures, and when it is 1,000 or less, the handleability of the curable resin composition is improved, which is preferable.
[0028] Examples of commercially available component (A-2) include, but are not limited to, those commercially available under the trade name jER from Mitsubishi Chemical Corporation (e.g., jER806, jER806H, jER807, jER4005P, jER4007P, jER4010P), those commercially available under the trade name DER from Olin Epoxy Co. (e.g., DER 334), those commercially available under the trade name ADEKA RESIN from ADEKA Corporation (e.g., EP-4901, EP-4901E), and those commercially available under the trade name EPICLON from DIC Corporation (e.g., EPICLON 830).
[0029] (Aliphatic Polybasic Acid-Modified Epoxy Resin (A-3)) The present curable resin composition may contain component (A-3) as component (A). When the present curable resin composition contains component (A-3) as component (A), the content of component (A-3) in component (A) is preferably more than 0% by mass and less than 3.0% by mass, more preferably more than 0% by mass and 2.0% by mass or less, and even more preferably more than 0% by mass and 1.0% by mass or less, based on 100% by mass of component (A). The content of component (A-3) in component (A) may be 0% by mass. In other words, the present curable resin composition does not have to contain component (A-3) as component (A). Since a curable resin composition can be provided in which the resulting cured product has an excellent elastic modulus in a high-temperature environment, the curable resin composition preferably does not contain (1) component (A-3) as component (A), or contains (2) more than 0 mass % and less than 3.0 mass % of component (A-3) relative to 100 mass % of component (A), as component (A).
[0030] In this specification, the term "aliphatic polybasic acid modified epoxy resin" refers to a compound obtained by subjecting an aliphatic polybasic acid or the like to an addition reaction with an epoxy resin.
[0031] Examples of aliphatic polybasic acids to be addition reacted with the epoxy resin include unsaturated polycarboxylic acids or anhydrides thereof that do not have an aromatic ring, such as maleic acid, maleic anhydride, fumaric acid, itaconic acid, itaconic anhydride, and citraconic acid; and saturated polycarboxylic acids or anhydrides thereof that do not have an aromatic ring, such as tetrahydrophthalic acid, tetrahydrophthalic anhydride, hexahydrophthalic acid, hexahydrophthalic anhydride, cyclohexanedicarboxylic acid, succinic acid, malonic acid, glutaric acid, adipic acid, azelaic acid, sebacic acid, 1,12-dodecanoic diacid, dimer acid, and trimer acid. However, the present invention is not limited to these, and commonly used aliphatic polybasic acids can be used. Dimer acid is particularly preferred because the resulting cured product has excellent vibration-damping properties.
[0032] As used herein, the term "dimer acid" refers to a dimer of an unsaturated fatty acid having 18 carbon atoms. Examples of the fatty acid having 18 carbon atoms include oleic acid, linoleic acid, and linolenic acid.
[0033] As the epoxy resin to be subjected to the addition reaction of the aliphatic polybasic acids, various epoxy resins can be used. Examples of such epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AD type epoxy resins, bisphenol S type epoxy resins, glycidyl ester type epoxy resins, glycidylamine type epoxy resins, novolac type epoxy resins, glycidyl ether type epoxy resins of bisphenol A propylene oxide adducts, hydrogenated bisphenol A (or F) type epoxy resins, fluorinated epoxy resins, flame retardant epoxy resins such as glycidyl ether of tetrabromobisphenol A, p-oxybenzoic acid glycidyl ether ester type epoxy resins, m-aminophenol type epoxy resins, diaminodiphenylmethane type epoxy resins, various alicyclic epoxy resins, N,N-diglycidylaniline, N,N-diglycidyl-o-toluidine, triglycidyl isocyanurate, divinylbenzene dioxide, resorcinol diglycidyl ether, polyalkylene glycol diglycidyl ether, and glycol diglycidyl ether. However, the epoxy resins are not limited to these, and commonly used epoxy resins can be used.
[0034] Component (A-3) is not particularly limited as long as it is an addition reaction product between the various aliphatic polybasic acids and the epoxy resin. Specific examples of component (A-3) include dimer acid-modified epoxy resins, hydrogenated dimer acid-modified epoxy resins, and trimer acid-modified epoxy resins. Dimer acid-modified epoxy resins, which are addition reaction products of a dimer of tall oil fatty acid (dimer acid) and a bisphenol A-type epoxy resin, as described in International Publication No. 2010-098950, are preferred because they are readily available and the resulting cured product has excellent vibration-damping properties. As component (A-3), one of these compounds may be used alone, or two or more may be used in combination.
[0035] Component (A-3) preferably contains a dimer acid-modified epoxy resin because it is readily available and the resulting cured product has superior vibration-damping properties. The curable resin composition preferably contains 80 mass% or more of the dimer acid-modified epoxy resin, based on a total amount (100 mass%) of component (A-3), more preferably 90 mass% or more, even more preferably 95 mass% or more, and particularly preferably 100 mass%.
[0036] The epoxy equivalent of component (A-3) is not particularly limited, but is preferably 250 to 800, more preferably 300 to 700, and even more preferably 380 to 500. When the epoxy equivalent of component (A-3) is 250 or more, there is an advantage that the obtained cured product has excellent vibration damping properties, and when it is 800 or less, the handleability of the curable resin composition is improved, which is preferable.
[0037] (Other Epoxy Resins) The curable resin composition may contain, as component (A), an epoxy resin (other epoxy resin) other than the above components (A-1) to (A-3). Examples of other epoxy resins include rubber-modified epoxy resins, bisphenol AD-type epoxy resins, bisphenol S-type epoxy resins, glycidyl ester-type epoxy resins, glycidyl amine-type epoxy resins, novolac-type epoxy resins, glycidyl ether epoxy resins of bisphenol A propylene oxide adducts, hydrogenated bisphenol A (or F)-type epoxy resins, fluorinated epoxy resins, flame-retardant epoxy resins such as glycidyl ether of tetrabromobisphenol A, p-oxybenzoic acid glycidyl ether ester-type epoxy resins, m-aminophenol-type epoxy resins, diaminodiphenylmethane-based epoxy resins, various alicyclic epoxy resins, N,N-diglycidyl aniline, N,N-diglycidyl-o-toluene. Examples include ethylenediamine, triglycidyl isocyanurate, divinylbenzene dioxide, resorcinol diglycidyl ether, polyalkylene glycol diglycidyl ether, glycol diglycidyl ether, diglycidyl esters of aliphatic polybasic acids, glycidyl ethers of dihydric or higher polyhydric aliphatic alcohols such as glycerin, epoxidized products of unsaturated polymers such as chelate-modified epoxy resins, urethane-modified epoxy resins, hydantoin-type epoxy resins, and petroleum resins, amino-containing glycidyl ether resins, and epoxy compounds obtained by addition reaction of the above-mentioned epoxy resins with bisphenol A (or F) or polybasic acids, but are not limited to these, and commonly used epoxy resins can be used.
[0038] When the present curable resin composition contains another epoxy resin as component (A), the content of the other epoxy resin in component (A) is not particularly limited, but is preferably 0.0 mass % to 20.0 mass %, more preferably 0.1 mass % to 10.0 mass %, and even more preferably 1.0 mass % to 5.0 mass %, relative to 100 mass % of component (A).
[0039] <Dicyandiamide (B)> The present curable resin composition contains component (B). In the present curable resin composition, dicyandiamide, which is component (B), can function as a curing agent that cures the curable resin composition. Dicyandiamide does not exhibit a curing action at temperatures below 100°C, or, even if it does exhibit a curing action, the curing reaction proceeds very slowly. On the other hand, when heated to a temperature of 100°C or higher (preferably 120°C), dicyandiamide exhibits a rapid curing action and can rapidly cure the curable resin composition. Due to these physical properties, dicyandiamide is sometimes referred to as a latent curing agent.
[0040] The curable resin composition contains 3.5 to 19.0 parts by mass of component (B) per 100 parts by mass of component (A), preferably 3.5 to 18.0 parts by mass, more preferably 4.0 to 16.0 parts by mass, more preferably 4.5 to 14.0 parts by mass, even more preferably 5.0 to 12.0 parts by mass, even more preferably 5.5 to 10.0 parts by mass, and particularly preferably 6.0 to 8.0 parts by mass. When the content of component (B) in the curable resin composition is (1) 3.5 parts by mass or more per 100 parts by mass of component (A), there is an advantage that the cured product obtained by curing the curable resin composition at low temperature has sufficient adhesive strength, and when (b) 19.0 parts by mass or less, there is an advantage that the storage stability of the curable resin composition is good and the resulting cured product has good moist heat resistance.
[0041] <Polymer particles (C) having a core-shell structure> The curable resin composition preferably contains polymer particles (C) having a core-shell structure (hereinafter, sometimes referred to as "component (C)") in addition to the above-mentioned components (A) and (B). When the curable resin composition contains component (C), it has the advantage of being able to provide a cured product (e.g., an adhesive layer) that is excellent in impact peel adhesion and adhesive strength.
[0042] In this specification, polymer particles having a core-shell structure refer to particles in which a layer structure is formed by a core layer made of a core polymer and a shell layer made of a shell polymer.
[0043] The structure of component (C) is not particularly limited as long as it has at least one core layer and at least one shell layer, and it can also have a three-layer or more structure including an intermediate layer covering the core layer and / or a shell layer further covering this intermediate layer. Furthermore, in component (C), the core layer and the shell layer do not have to form a complete layer structure. That is, the shell layer only needs to cover at least a portion of the core layer, and does not have to cover the entire core layer. Furthermore, a portion of the shell polymer constituting the shell layer may penetrate into the core layer.
[0044] In component (C), it is preferable that the shell polymer and core polymer are substantially chemically bonded (e.g., graft-bonded). Component (C) is more preferably a core-shell polymer particle obtained by graft polymerizing a graft-copolymerizable monomer (shell monomer) onto the core layer (core polymer) in the presence of the core layer to form a shell layer. Such a polymerization operation can be carried out, for example, by adding the shell monomer to a latex of the core polymer prepared in an aqueous polymer latex state and polymerizing the resulting polymer. Component (C) obtained by such an operation may have a structure comprising a core layer present within the core layer and at least one shell layer graft-polymerized onto the surface of the core layer, surrounding or partially covering the core layer.
[0045] Each layer that may contain component (C) will be specifically described below.
[0046] <<Core Layer>> The core layer of component (C) is preferably an elastic core layer having rubber properties in order to enhance the toughness of the cured product of the composition.
[0047] The core layer preferably contains a diene rubber because it provides a high toughness-improving effect on the resulting cured product, a high impact peel adhesion-improving effect on the resulting cured product, and is less likely to experience viscosity increases over time due to swelling of the core layer due to its low affinity with component (A). The core layer preferably contains a (meth)acrylate rubber because a wide range of polymer compositions can be designed by combining a variety of monomers. Furthermore, to improve low-temperature impact resistance without reducing the heat resistance of the cured product, the core layer preferably contains an organosiloxane rubber. In other words, the core layer preferably contains one or more rubbers selected from the group consisting of diene rubbers, (meth)acrylate rubbers, and organosiloxane rubbers.
[0048] (Diene Rubber) The diene rubber is preferably a polymer containing 50% by mass to 100% by mass of structural units derived from at least one monomer selected from the group consisting of conjugated diene monomers (hereinafter also referred to as conjugated diene units), and 0% by mass to 50% by mass of structural units derived from a vinyl monomer other than a conjugated diene monomer copolymerizable with the conjugated diene monomer.
[0049] Examples of the conjugated diene monomer include 1,3-butadiene, isoprene (2-methyl / 1,3-butadiene), and 2-chloro-1,3-butadiene.
[0050] These conjugated diene monomers may be used alone or in combination of two or more.
[0051] The content of the conjugated diene units in the core layer is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and even more preferably 90% by mass to 100% by mass, based on 100% by mass of all structural units constituting the core layer. When the content of the conjugated diene units in the core layer is 50% by mass or more, the impact peel adhesion of the resulting cured product can be improved.
[0052] Examples of vinyl monomers other than conjugated diene monomers copolymerizable with conjugated diene monomers include vinyl arenes such as styrene, α-methylstyrene, monochlorostyrene, and dichlorostyrene; vinyl carboxylic acids such as acrylic acid and methacrylic acid; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl halides such as vinyl chloride, vinyl bromide, and chloroprene; vinyl acetate; alkenes such as ethylene, propylene, butylene, and isobutylene; and polyfunctional monomers such as diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene.
[0053] These vinyl monomers may be used alone or in combination of two or more. Styrene is particularly preferred.
[0054] Among diene rubbers, the core layer more preferably contains butadiene rubber, which is a homopolymer of 1,3-butadiene, and / or butadiene / styrene rubber, which is a copolymer of 1,3-butadiene and styrene, from the viewpoints of a greater effect of improving the toughness of the resulting cured product, a greater effect of improving the impact peel adhesion of the resulting cured product, and a lower affinity with component (A) making it less likely that the viscosity will increase over time due to swelling of the core layer. It is more preferable that the core layer is (consisting only of) butadiene rubber and / or butadiene / styrene rubber, even more preferable that it contains butadiene rubber, and particularly preferable that it is (consisting only of) butadiene rubber. Furthermore, butadiene / styrene rubber is preferable because it can enhance the transparency of the resulting cured product by adjusting the refractive index.
[0055] ((Meth)acrylate Rubber) The (meth)acrylate rubber is preferably a polymer obtained by polymerizing a monomer mixture containing 50% by mass to 100% by mass of structural units (hereinafter also referred to as (meth)acrylate units) derived from at least one monomer selected from the group consisting of (meth)acrylate monomers, and 0% by mass to 50% by mass of structural units derived from vinyl monomers other than (meth)acrylate monomers that are copolymerizable with the (meth)acrylate monomers. In this specification, "(meth)acrylate" means acrylate and / or methacrylate.
[0056] Examples of the (meth)acrylate monomer include: (i) alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and behenyl (meth)acrylate; (ii) aromatic ring-containing (meth)acrylates such as phenoxyethyl (meth)acrylate and benzyl (meth)acrylate; and (iii) hydroxyalkyl (meth)acrylates. (iv) glycidyl (meth)acrylates such as glycidyl (meth)acrylate and glycidyl alkyl (meth)acrylate; (v) alkoxyalkyl (meth)acrylates; (vi) allyl alkyl (meth)acrylates such as allyl (meth)acrylate and allyl alkyl (meth)acrylate; (vii) polyfunctional (meth)acrylates such as monoethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, and the like.
[0057] Examples of hydroxyalkyl (meth)acrylates include hydroxy linear alkyl (meth)acrylates (particularly, hydroxy linear C1-6 alkyl (meth)acrylates) such as 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; caprolactone-modified hydroxy (meth)acrylates; hydroxy branched alkyl (meth)acrylates such as methyl α-(hydroxymethyl)acrylate and ethyl α-(hydroxymethyl)acrylate; and hydroxyl group-containing (meth)acrylates such as mono(meth)acrylates of polyester diols (particularly saturated polyester diols) obtained from divalent carboxylic acids (such as phthalic acid) and dihydric alcohols (such as propylene glycol).
[0058] These (meth)acrylate monomers may be used alone or in combination of two or more. Preferred (meth)acrylate monomers are ethyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.
[0059] Examples of vinyl monomers copolymerizable with (meth)acrylate monomers other than (meth)acrylate monomers include (i) vinyl arenes such as styrene, α-methylstyrene, monochlorostyrene, and dichlorostyrene; (ii) vinyl carboxylic acids such as acrylic acid and methacrylic acid; (iii) vinyl cyanides such as acrylonitrile and methacrylonitrile; (iv) vinyl halides such as vinyl chloride, vinyl bromide, and chloroprene; (v) vinyl acetate; (vi) alkenes such as ethylene, propylene, butylene, and isobutylene; and (vii) polyfunctional monomers such as diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene.
[0060] The vinyl monomer other than the (meth)acrylate monomer copolymerizable with the (meth)acrylate monomer may be used alone or in combination of two or more. Styrene is particularly preferred because it can easily increase the refractive index.
[0061] (Organosiloxane-Based Rubber) Examples of the organosiloxane-based rubber include (i) polysiloxane-based polymers composed of alkyl or aryl di-substituted silyloxy units, such as dimethylsilyloxy, diethylsilyloxy, methylphenylsilyloxy, diphenylsilyloxy, and dimethylsilyloxy-diphenylsilyloxy; and (ii) polysiloxane-based polymers composed of alkyl or aryl mono-substituted silyloxy units, such as organohydrogensilyloxy in which some of the alkyl groups in the side chains are substituted with hydrogen atoms.
[0062] These polysiloxane-based polymers may be used singly or in combination of two or more. Among these, dimethylsilyloxy, methylphenylsilyloxy, and dimethylsilyloxy-diphenylsilyloxy are preferred because they can impart heat resistance to the cured product, and dimethylsilyloxy is most preferred because it is easily available.
[0063] In order to enhance the toughness of the resulting cured product, the glass transition temperature of the core layer is preferably 0°C or lower, more preferably -20°C or lower, even more preferably -40°C or lower, and particularly preferably -60°C or lower.
[0064] The volume average particle diameter of the core layer is not particularly limited, but is preferably 0.03 μm to 2 μm, more preferably 0.05 μm to 1 μm, more preferably 0.12 μm to 0.50 μm, more preferably 0.12 μm to 0.28 μm, and even more preferably 0.14 μm to 0.25 μm. When the volume average particle diameter of the core layer is within this range, the core layer can be produced stably, and the cured product can have good heat resistance and impact resistance. The method for measuring the volume average particle diameter of the core layer will be described in detail in the Examples below.
[0065] The core layer may have a single layer structure or a multi-layer structure consisting of layers having rubber elasticity. When the core layer has a multi-layer structure, the polymer compositions of the layers may be different from each other within the ranges disclosed above.
[0066] In one embodiment of the present invention, an intermediate layer, for example, as described in paragraphs
[0046] to
[0049] of WO2016-163491, can be provided between the core layer and the shell layer.
[0067] <Shell Layer> The shell layer is a polymer obtained by polymerizing a shell monomer (a monomer for forming the shell layer). The polymer constituting the shell layer (shell polymer) plays a role of improving the compatibility between component (C) and component (A) and enabling component (C) to be dispersed in the form of primary particles in the curable resin composition and / or a cured product obtained by curing the curable resin composition.
[0068] As the shell monomer, one type of monomer may be used alone, or two or more types of monomers may be used in combination. When the shell monomer contains two or more types of monomers, the composition of the shell monomer, i.e., the types and content ratios of the monomers contained in the shell monomer, are not particularly limited. From the viewpoint of compatibility and dispersibility in the curable resin composition of component (C), the shell monomer is preferably an aromatic vinyl monomer, a vinyl cyan monomer, or a (meth)acrylate monomer, and more preferably a (meth)acrylate monomer. In particular, the shell monomer preferably contains methyl methacrylate.
[0069] In other words, the type and content ratio of the structural units contained in the shell layer are not particularly limited. From the viewpoint of compatibility and dispersibility of component (C) in the present curable resin composition, the shell layer preferably contains structural units derived from one or more monomers selected from the group consisting of aromatic vinyl monomers, vinylcyan monomers, and (meth)acrylate monomers, and more preferably contains structural units derived from (meth)acrylate monomers. In particular, the shell layer preferably contains structural units derived from metal methacrylate.
[0070] In the shell layer, the structural units derived from one or more monomers selected from the group consisting of aromatic vinyl monomers, vinylcyan monomers, and (meth)acrylate monomers preferably account for 10.0% by mass to 99.5% by mass in total, based on 100% by mass of the shell layer (shell polymer), more preferably 50.0% by mass to 99.0% by mass, even more preferably 65.0% by mass to 98.0% by mass, particularly preferably 67.0% by mass to 80.0% by mass, and most preferably 67.0% by mass to 85.0% by mass.
[0071] Specific examples of the aromatic vinyl monomer include styrene, α-methylstyrene, p-methylstyrene, and vinylbenzenes such as divinylbenzene.
[0072] Specific examples of the vinylcyan monomer include acrylonitrile and methacrylonitrile.
[0073] Specific examples of the (meth)acrylate monomer are the same as those explained in the section "Core Layer" above, and therefore, the explanation therefor is omitted here.
[0074] In order to maintain a good dispersion state of component (C) without aggregation in the present curable resin composition and in a cured product obtained by curing the present curable resin composition, the shell layer preferably has a structural unit derived from a reactive group-containing monomer from the viewpoint of chemically bonding component (C) and component (A). In other words, the shell layer of component (C) preferably contains a reactive group.
[0075] The reactive group contained in the shell layer of component (C) is preferably at least one selected from the group consisting of, for example, an epoxy group, an oxetane group, a hydroxyl group, an amino group, an imide group, a carboxylic acid group, a carboxylic acid anhydride group, a cyclic ester, a cyclic amide, a benzoxazine group, and a cyanate ester group.
[0076] The reactive group in the shell layer of component (C) is preferably an epoxy group, since the resulting cured product has excellent adhesive strength and impact peel adhesion. In other words, the shell layer of component (C) preferably has a structural unit derived from a monomer having an epoxy group, i.e., preferably has an epoxy group.
[0077] Specific examples of the monomer having an epoxy group include glycidyl group-containing vinyl monomers such as glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, and allyl glycidyl ether.
[0078] When the shell layer of component (C) contains epoxy groups, the content of epoxy groups in the shell layer of component (C) relative to the total mass of the shell layer is preferably more than 0 mmol / g but not more than 2.0 mmol / g, more preferably 0.1 mmol / g to 2.0 mmol / g or more, and even more preferably 0.3 mmol / g to 1.5 mmol / g, from the viewpoints of the adhesive strength and impact peel adhesion of the resulting cured product and the storage stability of the composition. This configuration suppresses aggregation of component (C), allowing component (C) to be dispersed in the cured product in the state of primary particles, thereby improving the adhesive strength and impact peel adhesion of the cured product.
[0079] The monomer having an epoxy group is preferably used to form the shell layer, and more preferably used only to form the shell layer. In other words, it is preferable that the core layer and the intermediate layer do not have an epoxy group.
[0080] In one embodiment of the present invention, from the viewpoint of the storage stability of the curable resin composition, it is preferable that the shell layer of component (C) does not have an epoxy group.
[0081] Specific examples of the hydroxyl group-containing monomer from which the reactive group contained in the shell layer of component (C) is derived include the above-mentioned hydroxyalkyl (meth)acrylates.
[0082]
[0033] When the shell layer contains a structural unit derived from a polyfunctional monomer having two or more radically polymerizable double bonds, swelling of component (C) in the curable resin composition can be prevented, and the viscosity of the curable resin composition is reduced, improving handleability, which is preferable. On the other hand, from the viewpoint of improving the toughness and impact peel adhesion of the resulting cured product, it is preferable that the shell layer does not contain a structural unit derived from a polyfunctional monomer having two or more radically polymerizable double bonds.
[0083] Specific examples of the polyfunctional monomer do not include conjugated diene monomers such as butadiene, and include allyl alkyl (meth)acrylates such as allyl (meth)acrylate and allyl alkyl (meth)acrylate; allyloxyalkyl (meth)acrylates; polyfunctional (meth)acrylates having two or more (meth)acrylic groups such as (poly)ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, and tetraethylene glycol di(meth)acrylate; diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene.
[0084] Among these polyfunctional monomers, allyl methacrylate and triallyl isocyanurate are preferred.
[0085] In one embodiment of the present invention, the shell layer of component (C) is preferably a polymer consisting of, for example, the following structural units: (a) 0% by mass to 50% by mass (preferably 1% by mass to 50% by mass, more preferably 2% by mass to 48% by mass) of structural units derived from an aromatic vinyl monomer (particularly preferably styrene), (b) 0% by mass to 50% by mass (preferably 0% by mass to 30% by mass, more preferably 10% by mass to 25% by mass) of structural units derived from a vinylcyan monomer (particularly preferably acrylonitrile), (c) (meth)acrylate and (d) 1% to 50% by mass (preferably 2% to 35% by mass, more preferably 3% to 20% by mass) of structural units derived from a monomer having an epoxy group (particularly glycidyl methacrylate). However, in the shell layer of component (C), the total of (i) structural units derived from an aromatic vinyl monomer, structural units derived from a vinylcyan monomer, structural units derived from a (meth)acrylate monomer, and structural units derived from a monomer having an epoxy group is 100% by mass, and (ii) 0% by mass of a certain structural unit means that the shell layer of component (C) may not contain that structural unit.
[0086] The above-mentioned monomer components may be used alone or in combination of two or more. The shell layer of component (C) may contain a constituent unit derived from a monomer other than the above-mentioned monomers.
[0087] The shell layer of component (C) may have a single-layer structure or a multi-layer structure. When the shell layer of component (C) has a multi-layer structure, the polymer compositions of the individual layers may be different from each other within the above range.
[0088] <Volume Average Particle Diameter (Mv) of Component (C)> The volume average particle diameter (Mv) of component (C) is not particularly limited, but from the viewpoint of industrial productivity and workability of the curable resin composition, it is preferably 0.01 μm to 2.00 μm, more preferably 0.03 μm to 0.60 μm, more preferably 0.05 μm to 0.40 μm, more preferably 0.10 μm to 0.30 μm, more preferably 0.15 μm to 0.30 μm, more preferably 0.16 μm to 0.28 μm, more preferably 0.17 μm to 0.27 μm, and even more preferably 0.18 μm to 0.25 μm. When the volume average particle diameter (Mv) of component (C) is (a) 0.01 μm or more, the viscosity of the curable resin composition is low, resulting in good workability, and when it is (b) 2.00 μm or less, the polymerization time of component (C) is short, resulting in high industrial productivity. The method for measuring the volume average particle diameter (Mv) of component (C) will be described in detail in the Examples below.
[0089] Component (C) is preferably dispersed in the curable resin composition in the form of primary particles. In this specification, "component (C) is dispersed in the form of primary particles" (hereinafter also referred to as "primary dispersion") means that multiple particles of component (C) are dispersed substantially independently (without contact) with each other, and this dispersion state can be confirmed, for example, by dissolving a part of the curable resin composition in a solvent such as methyl ethyl ketone and subjecting the resultant to a particle size measurement device using laser light scattering to measure the particle size of component (C) in the curable resin composition.
[0090] Furthermore, the term "stable dispersion" of component (C) means a state in which component (C) is steadily dispersed in the continuous layer under normal conditions for a long period of time without aggregation, separation, or precipitation. It is also preferable that the distribution of component (C) in the continuous layer does not change substantially, and that the "stable dispersion" can be maintained even when these compositions are heated within a safe range to reduce the viscosity and then stirred.
[0091] As component (C), one type of core-shell polymer particles may be used alone, or two or more types of core-shell polymer particles may be used in combination.
[0092] <Method for producing component (C)> (Method for producing core layer) The core layer constituting component (C) can be formed by polymerizing a core monomer by a known polymerization method, for example, emulsion polymerization, suspension polymerization, microsuspension polymerization, etc. Specific examples of the emulsion polymerization method, suspension polymerization method, and microsuspension polymerization method include those described in WO 2005 / 028546 and WO 2006 / 070664, as appropriate.
[0093] (Method of Forming Shell Layer and Intermediate Layer) The intermediate layer constituting component (C) can be formed by polymerizing the intermediate layer-forming monomer by known radical polymerization. When the rubber elastic material constituting the core layer is obtained as an emulsion, the intermediate layer-forming monomer is preferably polymerized by emulsion polymerization.
[0094] The shell layer constituting component (C) can be formed by polymerizing a shell monomer by known radical polymerization. When the core layer or the polymer particle precursor constituted by coating the core layer with an intermediate layer is obtained as an emulsion, it is preferable to polymerize the shell monomer by emulsion polymerization. As the emulsion polymerization method, for example, the method described in WO 2005 / 028546 can be appropriately used.
[0095] In emulsion polymerization, an emulsifier (dispersant) is used. Examples of the emulsifier include (i) (i-1) various acids such as alkyl or aryl sulfonic acids typified by dioctylsulfosuccinic acid and dodecylbenzenesulfonic acid; alkyl or aryl ether sulfonic acids; alkyl or aryl sulfuric acids typified by dodecyl sulfate; alkyl or aryl ether sulfuric acids; alkyl or aryl substituted phosphoric acids; alkyl or aryl ether substituted phosphoric acids; N-alkyl or aryl sarcosinic acids typified by dodecyl sarcosinic acid; alkyl or aryl carboxylic acids typified by oleic acid and stearic acid; and alkyl or aryl ether carboxylic acids; as well as (i-2) anionic emulsifiers (dispersants) such as alkali metal salts or ammonium salts of these acids; (ii) nonionic emulsifiers (dispersants) such as alkyl or aryl substituted polyethylene glycol; and (iii) dispersants such as polyvinyl alcohol, alkyl-substituted cellulose, polyvinylpyrrolidone, and polyacrylic acid derivatives.
[0096] These emulsifiers (dispersants) may be used alone or in combination of two or more.
[0097] It is preferable to use a small amount of emulsifier (dispersant) within a range that does not impair the dispersion stability of the aqueous latex of polymer particles. Furthermore, the higher the water solubility of the emulsifier (dispersant), the more preferable it is. High water solubility makes it easy to wash off the emulsifier (dispersant) with water, and can easily prevent adverse effects on the final cured product.
[0098] When emulsion polymerization is employed, peroxides (for example, organic peroxides), chain transfer agents, surfactants, and the like may be used as needed.
[0099] The polymerization conditions such as polymerization temperature, pressure, deoxidation, etc., may be within known ranges.
[0100] In order to achieve an excellent balance between the storage stability of the curable resin composition and the toughness-improving effect of the resulting cured product, the content of component (C) in the present curable resin composition is preferably 1 to 100 parts by mass, more preferably 5 to 90 parts by mass, even more preferably 10 to 80 parts by mass, still more preferably 20 to 70 parts by mass, and particularly preferably 30 to 60 parts by mass, relative to 100 parts by mass of component (A).
[0101] <Curing Accelerator (D)> The curable resin composition preferably contains a curing accelerator (D). In this specification, the "curing accelerator (D)" may be referred to as "component (D)." Component (D) is a compound that functions as a catalyst for promoting the reaction (i.e., curing reaction) between the epoxy group in component (A) and the epoxide-reactive group in component (B) and components other than component (A) contained in the curable resin composition.
[0102] The component (D) is not particularly limited as long as it has the above-mentioned catalytic action, and examples thereof include: (a) ureas such as 3-(3,4-dichlorophenyl)-1,1-dimethylurea, p-chlorophenyl-N,N-dimethylurea (trade name: Monuron), 3-phenyl-1,1-dimethylurea (trade name: Fenuron), 3,4-dichlorophenyl-N,N-dimethylurea (trade name: Diuron), N-(3-chloro-4-methylphenyl)-N',N'-dimethylurea (trade name: Chlortoluron), and 1,1-dimethylphenylurea (trade name: Dyhard); (b) benzyldimethylamine, 2,4,6-tris(dichlorophenyl)-N,N-dimethylurea (trade name: Diuron), and 1,1-dimethylphenylurea (trade name: Dyhard); (c) tertiary amines such as C1-C12 alkylene imidazole, N-arylimidazole, 2-methylimidazole, 2-ethyl-2-methylimidazole, N-butylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, and addition products of epoxy resins and imidazole; and (d) 6-caprolactam. Component (D) may be encapsulated in a microcapsule or may be a latent catalyst that becomes active only at elevated temperatures. Component (D) may be used alone or in combination of two or more of these.
[0103] The present curable resin composition preferably contains 0.1 to 10.0 parts by mass of component (D) relative to 100 parts by mass of component (A), more preferably 0.2 to 5.0 parts by mass, even more preferably 0.5 to 3.0 parts by mass, and particularly preferably 0.8 to 2.0 parts by mass. When the content of component (D) is (a) 0.1 parts by mass or more relative to 100 parts by mass of epoxy resin (A), the curability of the present curable resin composition is good, and when (b) 10.0 parts by mass or less, the storage stability of the present curable resin composition is good, which has the advantage of being easy to handle.
[0104] <Inorganic Filler> The present curable resin composition preferably contains an inorganic filler. When the present curable resin composition contains an inorganic filler, the obtained cured product has the effect of having superior rigidity at high temperatures.
[0105] Examples of inorganic fillers include silicic acid and / or silicates such as dry silica, wet silica, aluminum silicate, magnesium silicate, and calcium silicate; reinforcing fillers such as wollastonite, talc, dolomite, and carbon black; and calcium oxide, heavy calcium carbonate, colloidal calcium carbonate, magnesium carbonate, titanium oxide, ferric oxide, fine aluminum powder, zinc oxide, and activated zinc oxide. One of these inorganic fillers may be used alone, or two or more may be used in combination.
[0106] The dry silica is also called fumed silica. Examples of fumed silica include hydrophilic fumed silica with no surface treatment and hydrophobic fumed silica produced by chemically treating the silanol groups of hydrophilic fumed silica with silane or siloxane. From the viewpoint of dispersibility in component (A), hydrophobic fumed silica is preferred.
[0107] The content of the inorganic filler in the curable resin composition is preferably 1 to 300 parts by mass, more preferably 5 to 200 parts by mass, and even more preferably 10 to 150 parts by mass, per 100 parts by mass of component (A). When the content of the inorganic filler is within the above range, there is an advantage that the obtained cured product has even better rigidity and adhesive strength at high temperatures.
[0108] <Other Components> The curable resin composition may contain components (other components) other than the above-described components, as necessary. Examples of other components include a curing agent other than dicyandiamide, a phenolic compound, a blocked urethane, a reinforcing agent, calcium oxide, a radical-curing resin, a monoepoxide, a photopolymerization initiator, an expanding agent such as an azo-type chemical foaming agent or thermally expandable microballoons, fiber pulp such as aramid pulp, a colorant such as a pigment or dye, an extender pigment, an ultraviolet absorber, an antioxidant, a stabilizer (antigelling agent), a plasticizer, a leveling agent, an antifoaming agent, a silane coupling agent, an antistatic agent, a flame retardant, a lubricant, a viscosity reducer, a low-shrinkage agent, an organic filler, a thermoplastic resin, a desiccant, and a dispersant.
[0109] <Method for Producing Curable Resin Composition> The method for producing the curable resin composition is not particularly limited, and various methods can be used. Examples include a method in which component (C) obtained in an aqueous latex state is contacted with component (A) and then unnecessary components such as water are removed, and a method in which component (C) is extracted into an organic solvent, then mixed with component (A), and then the organic solvent is removed. Specifically, as such a production method, it is preferable to use the method described in WO 2005 / 028546. More specifically, the curable resin composition is preferably prepared by a production method including the following steps 1 to 3, in order. a first step in which an aqueous latex containing component (C) (specifically, a reaction mixture obtained after producing component (C) by emulsion polymerization) is mixed with an organic solvent having a solubility in water at 20°C of 5% by mass to 40% by mass, and then the mixture is further mixed with excess water to aggregate component (C); a second step in which the aggregated component (C) is separated and recovered from the liquid phase, and then mixed again with an organic solvent to obtain an organic solvent solution of polymer particles (B); and a third step in which the organic solvent solution of component (C) is further mixed with component (A), and then the organic solvent is distilled off.
[0110] The present curable resin composition can be obtained by mixing additional component (A), component (B), and, if necessary, component (D), an inorganic filler, and other components with the dispersion in which component (C) is dispersed in component (A) in the state of primary particles, obtained through the above-mentioned steps 1 to 3. Furthermore, this production method can obtain the present curable resin composition in which component (C) is dispersed in the state of primary particles. When the present curable resin composition is a composition in which component (C) is dispersed in component (A) in the state of primary particles, the obtained cured product has the advantage of excellent impact peel adhesion strength.
[0111] Alternatively, the present curable resin composition can be produced by redispersing powdery component (C) obtained by coagulating by a method such as salting out and then drying it in component (A) using a disperser having high mechanical shear force, such as a three-roll paint roll, a roll mill, or a kneader. In this case, component (C) can be efficiently dispersed in component (A) by applying mechanical shear force to components (A) and (C) at high temperature. When the present curable resin composition is produced by applying mechanical shear force using a disperser, the temperature at which component (C) is dispersed in component (A) (the temperature at which mechanical shear force is applied) is preferably 50°C to 200°C, more preferably 70°C to 170°C, even more preferably 80°C to 150°C, and particularly preferably 90°C to 120°C.
[0112] The curable resin composition of the present invention can be used as a one-component curable resin composition in which all components are blended in advance, sealed, and stored, and then cured by heating or light irradiation after application. Alternatively, the composition can be prepared as a two-component or multi-component curable resin composition, including a liquid A containing component (A) as the main component and further containing component (C), and a liquid C prepared separately from liquid A, containing component (B) and, optionally, component (D), and further containing component (C) as needed, and then mixed with liquid C before use. The curable resin composition of the present invention is particularly advantageous when used as a one-component curable resin composition.
[0113] When the present curable resin composition is a two-component or multi-component curable resin composition, component (C) may be contained in at least one of component A and component C. That is, component (C) may be contained only in component A, only in component C, or both in component A and component C.
[0114] (2-2. Adherend) An adherend according to one embodiment of the present invention (hereinafter, sometimes referred to as "the adherend") will be described in detail below. The "adherend" may also be referred to as a "substrate" or an "adhesion substrate."
[0115] Examples of materials for the adherend include wood, metal, plastic, glass, etc. More specifically, examples include (i) steel materials such as cold-rolled steel and hot-dip galvanized steel, (ii) aluminum materials such as aluminum and coated aluminum, and (iii) various plastic substrates such as general-purpose plastics, engineering plastics, and composite materials such as CFRP and GFRP.
[0116] In this manufacturing method, at least two adherends, i.e., a first adherend and a second adherend, are used. The first adherend and the second adherend in this manufacturing method may be made of the same type of material, or may be made of different types of material. It is preferable that at least one of the first adherend and the second adherend is made of a steel material, and more preferable that both are made of a steel material, because this has the advantages of being inexpensive, high-strength, and excellent in weldability and formability. That is, in one embodiment of the present invention, it is preferable that the first adherend and / or the second adherend is made of a steel material, and more preferable that both the first adherend and the second adherend are made of a steel material.
[0117] The thickness of the first and second adherends in this production method is not particularly limited, but is preferably 0.4 mm to 3.2 mm, more preferably 0.8 mm to 2.4 mm, and even more preferably 1.2 mm to 1.6 mm. The first and second adherends in this production method may have the same thickness or different thicknesses.
[0118] The average thickness (X) of the first and second adherends (hereinafter sometimes simply referred to as "(X)") is not particularly limited, but is preferably 0.4 mm to 3.2 mm, more preferably 0.8 mm to 2.4 mm, and even more preferably 1.2 mm to 1.6 mm. The average thickness (X) of the first and second adherends can be calculated based on the following formula: Average thickness (X) of the first and second adherends = (thickness of the first adherend + thickness of the second adherend) / 2.
[0119] (2-3. Step (i) (Laminating Step)) Step (i) in the present manufacturing method is a step of applying the present curable resin composition to a first adherend and then laminating a second adherend to the first adherend. At this time, the first adherend and the second adherend are laminated together so that the present curable resin composition applied to the first adherend is sandwiched between the first adherend and the second adherend. At this time, the curable resin composition sandwiched between the first adherend and the second adherend may partially protrude from the first adherend and / or the second adherend. Furthermore, the present curable resin composition may be applied to a second adherend as well as the first adherend, if necessary. Step (i) according to one embodiment of the present invention (hereinafter, sometimes referred to as "this step (i)") can also be said to be a step of obtaining a structure (hereinafter, sometimes referred to as "structure (i)") in which a first adherend, the curable resin composition, and a second adherend are laminated in this order.
[0120] In step (i), the method for applying the curable resin composition to the first adherend (and, if necessary, the second adherend) is not particularly limited, and any method can be used. For example, the curable resin composition can be applied to the first adherend by extruding the curable resin composition onto the first adherend in the form of a bead, monofilament, or swirl using a coating robot, by a mechanical coating method such as a caulking gun, by a jet spray method or a streaming method, or by other manual coating means.
[0121] In this step (i), the thickness of the curable resin composition in the resulting structure (i) is preferably adjusted so that the ratio (Y / X) of the thickness (Y) of the cured product obtained by curing the curable resin composition (hereinafter simply referred to as "(Y)") to the average thickness (X) of the first adherend and the second adherend is 0.5 to 10.0. The thickness of the curable resin composition in which the value of (Y / X) in the resulting cured product is 0.5 to 10.0 cannot be generally defined because it varies depending on the average thickness of the first adherend and the second adherend used, but is, for example, preferably 0.2 mm to 4 mm, more preferably 0.3 mm to 3 mm, and even more preferably 0.4 mm to 2 mm. In other words, in this step (i), it is preferable to adjust the thickness of the applied curable resin composition to the above range.
[0122] The method for adjusting the thickness of the curable resin composition in the obtained structure (i) is not particularly limited, and examples thereof include (1) a method in which the curable resin composition applied to the first adherend is stretched using a spatula or the like, or (2) a method in which, when bonding the second adherend to the first adherend, the curable resin composition is sandwiched between the two adherends, and the two adherends press and stretch the curable resin composition.
[0123] As described above, this step (i) preferably includes a step (thickness adjusting step) of adjusting the thickness of the curable resin composition in the obtained structure (i) so that the thickness of the cured product obtained by curing the curable resin composition becomes a desired thickness.
[0124] (2-4. Step (ii) (Curing Step)) Step (ii) in this production method is a step of curing the present curable resin composition present between the first adherend and the second adherend in the structure (i) obtained in step (i). By curing the present curable resin composition in step (ii), it is possible to obtain a laminate (hereinafter sometimes referred to as a "laminate") in which two adherends (the first adherend and the second adherend) are bonded together by a cured product obtained by curing the present curable resin composition.
[0125] In step (ii) according to one embodiment of the present invention (hereinafter sometimes referred to as "this step (ii)"), the curable resin composition in the structure (i) is cured by heating. Therefore, this step (ii) can also be said to be a "heating step" or a "heat curing step".
[0126] The curing temperature in step (ii) (the temperature at which the curable resin composition is heated) is 105°C to 145°C, preferably 115°C to 140°C, and more preferably 125°C to 135°C. The "curing temperature" refers to the ambient temperature of the space in which the curable resin composition is heated, and when step (ii) is performed using a baking oven, it refers to the set temperature of the baking oven. By setting the curing temperature in step (ii) to 145°C or less, it is possible to reduce the fuel required for heating, which can contribute to achieving carbon neutrality.
[0127] The curing time in step (ii) (the time for heating the curable resin composition) is 10 to 60 minutes, preferably 15 to 40 minutes, and more preferably 15 to 30 minutes. The "curing time" refers to the time for which the curable resin composition is maintained in a heating space, and when step (ii) is performed using a baking oven, refers to the time from when the structure (i) is placed in the baking oven until when it is removed. By keeping the curing time in step (ii) to 60 minutes or less, it is possible to reduce the fuel required for heating, which can contribute to achieving carbon neutrality.
[0128] In this specification, the heat curing of a curable resin composition containing an epoxy resin, which is carried out under conditions where the curing temperature is 145°C or less (105°C to 145°C) and the curing time is 60 minutes or less, as described above, is referred to as "low-temperature curing." This step (ii) can also be said to be a low-temperature curing step.
[0129] When the present curable resin composition is used as an automotive adhesive, in other words, when the present production method is used in the production of a vehicle body structure, it is preferable, from the viewpoint of shortening and simplifying the process, to apply the present curable resin composition to an automotive member as an adherend, and then further apply a coating such as electrodeposition coating, and bake and cure the coating while curing the present curable resin composition.
[0130] (2-5. Laminate and Cured Product) A laminate according to one embodiment of the present invention and a cured product in the laminate (a cured product obtained by curing the present curable resin composition) will be described in detail below. In this specification, the "laminate according to one embodiment of the present invention" may be referred to as the "present laminate," and the "cured product according to one embodiment of the present invention" may be referred to as the "present cured product."
[0131] <Ratio of Thickness of Cured Product to Thickness of Adherend> In the present laminate, the ratio (Y / X) of the thickness (Y) of the present cured product to the average thickness (X) of the first and second adherends is 0.5 to 10.0. By controlling (Y / X) to 0.5 to 10.0, in other words, by performing steps (i) and (ii) above so that (Y / X) is 0.5 to 10.0, it is possible to provide a laminate in which adherends are bonded by a cured product that has a high elastic modulus in a high-temperature environment, even when cured at low temperature. In the present laminate, (Y / X) is more preferably greater than 0.5 and not greater than 5.0, and even more preferably 0.7 to 3.0.
[0132] <Glass Transition Temperature of Cured Product> The glass transition temperature (Tg1) of the present cured product in Celsius is not particularly limited, but is preferably 120°C or higher, more preferably 122°C or higher, and even more preferably 125°C or higher, because this can reduce the decrease in elastic modulus of the cured product in a high-temperature environment. The method for measuring the glass transition temperature (Tg1) of the cured product is as described in the Examples. Tg1 can also be said to be the glass transition temperature in Celsius of the cured product obtained by low-temperature curing of the present curable resin composition, or the glass transition temperature in Celsius of the cured product in the laminate immediately after step (ii) (immediately after production of the laminate).
[0133] The glass transition temperature (Tg2) in Celsius of the cured product obtained by heat-curing the curable resin composition under sufficient heating conditions (herein, a curing temperature of 130°C and a curing time of 2 hours) is not particularly limited, but is preferably 20°C or higher, more preferably 50°C or higher, even more preferably 80°C or higher, still more preferably 100°C or higher, even more preferably 120°C or higher, and particularly preferably 130°C or higher. The method for measuring the glass transition temperature (Tg2) of the cured product is as described in the Examples. It can also be said that Tg2 is the glass transition temperature in Celsius of the cured product obtained by heat-curing the curable resin composition under sufficient heating conditions (herein, a curing temperature of 130°C and a curing time of 2 hours).
[0134] <Glass transition temperature attainment rate> The glass transition temperature attainment rate of a cured product is the ratio (Tg1 / Tg2) of the Celsius-based glass transition temperature (Tg1) of a cured product obtained by (1) low-temperature curing of a curable resin composition containing an epoxy resin, to (2) the Celsius-based glass transition temperature (Tg2) of a cured product obtained by heat-curing under sufficient heating conditions (herein, a curing temperature of 130°C and a curing time of 2 hours). The glass transition temperature attainment rate of a cured product can be calculated using the following formula: Glass transition temperature attainment rate (%) of a cured product = (Celsius-based glass transition temperature (Tg1) (°C) of a cured product obtained by curing a curable resin composition at a curing temperature of 130°C for a curing time of 20 minutes / Celsius-based glass transition temperature (Tg2) (°C) of a cured product obtained by curing a curable resin composition at a curing temperature of 130°C for a curing time of 120 minutes) × 100.
[0135] The crosslink density (curing conversion rate) of a cured product obtained by curing a curable resin composition containing an epoxy resin varies depending on the curing temperature and curing time. As a result, the glass transition temperature of a cured product obtained by curing a curable resin composition containing an epoxy resin also varies depending on the curing temperature and curing time. In particular, the inventors have found that when a curable resin composition is cured at low temperatures, the glass transition temperature of the resulting cured product tends to be significantly lower than when the curable resin composition is cured under sufficient heating conditions (e.g., a curing temperature of 130°C and a curing time of 2 hours). Note that when a curable resin composition is cured for a sufficiently long time, the curing reaction is completed (the curing conversion rate becomes 100% or nearly 100%) and the cured product comprising each composition reaches its own glass transition temperature. In this specification, "sufficient heating conditions" refers to heating conditions that complete the curing reaction. Furthermore, the glass transition temperature (Tg2) of a cured product obtained by heat curing under sufficient heating conditions can also be said to be the glass transition temperature of the cured product at the time the curing reaction is completed.
[0136] The present inventors have considered that this decrease in glass transition temperature during low-temperature curing is one of the reasons why the elastic modulus of the resulting cured product in a high-temperature environment decreases significantly when the curable resin composition is cured at low temperature. Conversely, the present inventors have considered that if the decrease in glass transition temperature during low-temperature curing can be suppressed, a cured product having a high elastic modulus in a high-temperature environment can be provided.
[0137] The glass transition temperature ratio (Tg1 / Tg2) is an index showing the degree of suppression of the decrease in glass transition temperature during low-temperature curing. The higher the Tg1 / Tg2, the more suppressed the decrease in glass transition temperature during low-temperature curing; in other words, the more suppressed the decrease in elastic modulus of the cured product in a high-temperature environment. Therefore, from the viewpoint of providing a cured product having a high elastic modulus even in a high-temperature environment, the glass transition temperature ratio (Tg1 / Tg2) of the cured product in the laminate obtained by this production method is preferably 80% or more, more preferably 81% or more, and even more preferably 83% or more. The glass transition temperature ratio (Tg1 / Tg2) of the cured product in the laminate can be measured by the method described in the Examples.
[0138] The rate at which the glass transition temperature is reached can be controlled by adjusting the composition of the curable resin composition (particularly the composition of the epoxy resin), the ratio between the thickness of the cured product and the thickness of the adherend, and the like.
[0139] <Storage modulus (E') at 120°C> The cured product has a high elastic modulus in a high-temperature environment. In this specification, the "elastic modulus at high temperature" of the cured product can be evaluated by the storage modulus E' of the cured product at 120°C. The storage modulus of the cured product at 120°C can be measured using a tensile mode dynamic viscoelasticity measurement at a frequency of, for example, 1 Hz.
[0140] The storage modulus of the present cured product at 120°C is preferably 0.07 GPa or more, more preferably 0.08 GPa or more, even more preferably 0.09 GPa or more, and particularly preferably 0.10 GPa or more. The higher the storage modulus of the cured product at 120°C, the better the elastic modulus of the cured product in a high-temperature environment. The upper limit of the storage modulus of the present cured product at 120°C is not particularly limited, but can be, for example, 5.0 GPa or less.
[0141] <Storage Modulus (E') at 100°C> In this specification, the "elastic modulus at high temperature" of a cured product can also be evaluated in terms of the storage modulus E' of the cured product at 100°C. The storage modulus of the cured product at 100°C can be measured by dynamic viscoelasticity measurement in tension mode at a frequency of, for example, 1 Hz.
[0142] The storage modulus at 100°C of the present cured product is preferably 1.05 GPa or more, more preferably 1.1 GPa or more, even more preferably 1.2 GPa or more, and particularly preferably 1.3 GPa or more. The higher the storage modulus at 100°C of the cured product, the better the elastic modulus of the cured product in a high-temperature environment. The upper limit of the storage modulus at 100°C of the present cured product is not particularly limited, but can be, for example, 5.0 GPa or less.
[0143] <Storage modulus (E') at 23°C> The cured product also has an excellent elastic modulus at room temperature. In this specification, the "elastic modulus at room temperature" of the cured product can be evaluated by the storage modulus E' of the cured product at 23°C. The storage modulus of the cured product at 23°C can be measured by dynamic viscoelasticity measurement in tension mode at a frequency of, for example, 1 Hz.
[0144] The storage modulus of the cured product at 23°C is preferably 1.0 GPa or more, more preferably 1.5 GPa or more, and even more preferably 2.0 GPa or more. The higher the storage modulus of the cured product at 23°C, the better the modulus of elasticity of the cured product at room temperature. There is no particular upper limit to the storage modulus at 23°C, but it can be, for example, 5.0 GPa or less.
[0145] The fact that the cured product obtained by low-temperature curing of a curable resin composition has a storage modulus at 23°C of 1.0 GPa or more and a glass transition temperature (Tg1) in Celsius of 120°C or more means that even when the cured product is cured at low temperature for a short time, the cured product has a high elastic modulus in a high-temperature environment and adheres to an adherend. Therefore, it is preferable that the cured product in the laminate obtained by this production method has a storage modulus at 23°C of 1.0 GPa or more and a glass transition temperature (Tg1) in Celsius of 120°C or more.
[0146] <Uses of Laminate> The present laminate can be suitably used, for example, for bonding components in the manufacture of automobile and vehicle (bullet train, train, etc.) bodies, aircraft, spacecraft, space stations, buildings, structures, wind power plants, etc., particularly for bonding components in the manufacture of vehicle body structures (more specifically, floor panels, center pillars, etc.). That is, in one embodiment of the present invention, there is provided a method for manufacturing a vehicle body structure that includes the present manufacturing method as one step.
[0147] 3. Others An embodiment of the present invention may include the following configuration.
[0148] [1] A method for producing a laminate in which a first adherend, a cured product obtained by curing a curable resin composition, and a second adherend are laminated in this order, the method comprising: a step (i) of applying the curable resin composition to the first adherend and laminating the second adherend to the first adherend (laminating step); and a step (ii) of curing the curable resin composition (curing step), wherein the curable resin composition is a mixture of an epoxy resin (A) and 3.5 to 19 parts by mass of dicyandiamide (B) per 100 parts by mass of the epoxy resin (A). 0 parts by mass, wherein the epoxy resin (A) contains 51% by mass to 100% by mass of an unmodified bisphenol A epoxy resin (A-1) relative to a total amount (100% by mass) of the epoxy resin (A), the curing temperature of the curable resin composition in the step (ii) is 105°C to 145°C, the curing time of the curable resin composition in the step (ii) is 10 minutes to 60 minutes, and the ratio (Y / X) of the thickness (Y) of the cured product to the average thickness (X) of the first adherend and the second adherend is 0.5 to 10.0.
[0149] [2] The method for producing a laminate according to [1], wherein the glass transition temperature attainment rate of the cured product is 80% or more; wherein the glass transition temperature attainment rate of the cured product is a value calculated by the following formula: glass transition temperature attainment rate of the cured product = (glass transition temperature (Tg1) (°C) in Celsius of the cured product obtained by curing the curable resin composition at a curing temperature of 130°C for a curing time of 20 minutes / glass transition temperature (Tg2) (°C) in Celsius of the cured product obtained by curing the curable resin composition under conditions of a curing temperature of 130°C for a curing time of 120 minutes) × 100.
[0150] [3] The method for producing a laminate according to [1] or [2], wherein the cured product has a storage modulus of 1 GPa or more at 23°C, and the storage modulus is a value obtained by measuring the cured product in a tensile mode in dynamic viscoelasticity measurement at a frequency of 1 Hz.
[0151] [4] The method for producing a laminate according to any one of [1] to [3], wherein the cured product has a storage modulus of 0.07 GPa or more at 120°C, and the storage modulus is a value obtained by measuring the storage modulus in a tensile mode of dynamic viscoelasticity measurement at a frequency of 1 Hz.
[0152] [5] The method for producing a laminate according to any one of [2] to [4], wherein the glass transition temperature (Tg1) of the cured product is 120°C or higher.
[0153] [6] The method for producing a laminate according to any one of [1] to [5], wherein the epoxy resin (A) does not contain an aliphatic polybasic acid-modified epoxy resin (A-3).
[0154] [7] The method for producing a laminate according to any one of [1] to [5], wherein the epoxy resin (A) contains an aliphatic polybasic acid-modified epoxy resin (A-3), and the content of the aliphatic polybasic acid-modified epoxy resin (A-3) in the epoxy resin is more than 0 mass% and less than 3 mass%.
[0155] [8] The method for producing a laminate according to any one of [1] to [7], wherein the first adherend and / or the second adherend is a steel plate.
[0156] [9] The method for producing a laminate according to any one of [1] to [8], wherein the curable resin composition further contains 1 part by mass to 100 parts by mass of polymer particles (C) having a core-shell structure including a core layer and a shell layer, relative to 100 parts by mass of the epoxy resin (A).
[0157]
[10] The method for producing a laminate according to any one of [1] to [9], wherein the curable resin composition further contains 0.1 to 15 parts by mass of a curing accelerator (D) relative to 100 parts by mass of the epoxy resin (A).
[0158]
[11] The method for producing a laminate according to [9], wherein the core layer contains at least one rubber selected from the group consisting of diene rubber, (meth)acrylate rubber, and organosiloxane rubber.
[0159]
[12] The method for producing a laminate according to [9] or
[11] , wherein the core layer is made of butadiene rubber and / or butadiene / styrene rubber.
[0160]
[13] The method for producing a laminate according to any one of
[10] to
[12] , wherein the shell layer contains a structural unit derived from one or more monomers selected from the group consisting of an aromatic vinyl monomer, a vinylcyan monomer, and a (meth)acrylate monomer.
[0161]
[14] A method for manufacturing a vehicle body structure, comprising the method for manufacturing the laminate according to any one of [1] to
[13] .
[0162] The following examples will explain one embodiment of the present invention in more detail, but the present invention is not limited to these examples.
[0163] [Materials] The materials used in the examples and comparative examples are shown below.
[0164] (Component (A)) Component (A-1): JER828 (manufactured by Mitsubishi Chemical, bisphenol A type epoxy resin that is liquid at room temperature, epoxy equivalent: 184 to 194) Component (A-2): JER807 (manufactured by Mitsubishi Chemical, bisphenol F type epoxy resin that is liquid at room temperature, epoxy equivalent: 160 to 175) Component (A-3): JER871 (manufactured by Mitsubishi Chemical, dimer acid modified epoxy resin, epoxy equivalent: 410 g / eq) (Other epoxy resins) HyPox RA840 (manufactured by CVC, rubber modified epoxy resin, epoxy equivalent: 350) (Component (B)) Dyhard 100S (manufactured by AlzChem, dicyandiamide) (Component (C)) As component (C), polymer particles prepared by the following method were used. As will be described later, component (C) was used in the form of a dispersion (M-1) in which the prepared polymer particles were dispersed in component (A) (component (A-1)).
[0165] 1. Formation of Core Layer Production Example 1-1: Preparation of Polybutadiene Rubber Latex (R-1) Into a 100 L pressure-resistant polymerization reactor, 200 parts by mass of deionized water, 0.03 parts by mass of tripotassium phosphate, 0.25 parts by mass of potassium dihydrogen phosphate, 0.002 parts by mass of disodium ethylenediaminetetraacetate (EDTA), 0.001 parts by mass of ferrous sulfate heptahydrate (FE), and 1.5 parts by mass of sodium dodecylbenzenesulfonate (SDS) as an emulsifier were charged. Next, the gas inside the pressure-resistant polymerization reactor was replaced with nitrogen while stirring the charged raw materials, thereby thoroughly removing oxygen from inside the pressure-resistant polymerization reactor. Thereafter, 100 parts by mass of butadiene (BD) was charged into the pressure-resistant polymerization reactor, and the temperature inside the pressure-resistant polymerization reactor was raised to 45 ° C. Next, 0.015 parts by mass of paramenthane hydroperoxide (PHP) was charged into the pressure-resistant polymerization reactor, followed by 0.04 parts by mass of sodium formaldehyde sulfoxylate (SFS) to initiate polymerization. Ten hours after the start of polymerization, the polymerization was terminated by devolatilization under reduced pressure to remove remaining monomers that had not been used in the polymerization. During the polymerization, PHP, EDTA, and FE were each added to the pressure-resistant polymerization reactor in desired amounts and at desired times. This polymerization procedure yielded a latex (R-1) containing a core layer (polybutadiene rubber particles) primarily composed of polybutadiene rubber. The volume average particle diameter of the polybutadiene rubber particles contained in the resulting latex was 0.10 μm.
[0166] Production Example 1-2: Preparation of Polybutadiene Rubber Latex (R-2) Into a 100 L pressure-resistant polymerization reactor, 7 parts by mass (solids) of the polybutadiene rubber latex (R-1) obtained in Production Example 1-1, 200 parts by mass of deionized water, 0.03 parts by mass of tripotassium phosphate, 0.002 parts by mass of EDTA, and 0.001 parts by mass of FE were charged. Next, while stirring the charged raw materials, the gas inside the pressure-resistant polymerization reactor was replaced with nitrogen, thereby sufficiently removing oxygen from inside the pressure-resistant polymerization reactor. Thereafter, 93 parts by mass of BD was charged into the pressure-resistant polymerization reactor, and the temperature inside the pressure-resistant polymerization reactor was raised to 45°C. Next, 0.02 parts by mass of PHP was charged into the pressure-resistant polymerization reactor, followed by 0.10 parts by mass of SFS, to initiate polymerization. Thirty hours after the start of polymerization, the polymerization was terminated by devolatilization under reduced pressure to remove remaining monomers that were not used in the polymerization. During the polymerization, PHP, EDTA, and FE were each added to the pressure-resistant polymerization reactor in desired amounts and at desired times. Through this polymerization procedure, a latex (R-2) containing a core layer (polybutadiene rubber particles) composed mainly of polybutadiene rubber was obtained. The volume average particle diameter of the polybutadiene rubber particles contained in the obtained latex was 0.20 μm.
[0167] 2. Preparation of Polymer Particles Having a Core-Shell Structure (Formation of Shell Layer) Production Example 2-1: Preparation of Core-Shell Polymer Latex (L-1) 262 parts by mass of the polybutadiene rubber latex (R-2) prepared in Production Example 1-2 (containing 87 parts by mass of polybutadiene rubber particles) and 57 parts by mass of deionized water were placed in a glass reactor. The glass reactor was equipped with a thermometer, a stirrer, a reflux condenser, a nitrogen inlet, and a monomer addition device. The gas in the glass reactor was replaced with nitrogen, and the raw materials placed in the reactor were stirred at 60°C while the nitrogen replacement was being carried out. Next, 0.004 parts by mass of EDTA, 0.001 parts by mass of FE, and 0.2 parts by mass of SFS were added to the glass reactor. Thereafter, a mixture of shell layer-forming monomers (1 part by mass of methyl methacrylate (MMA), 6 parts by mass of styrene (ST), 2 parts by mass of acrylonitrile (AN), and 4 parts by mass of glycidyl methacrylate (GMA)) and 0.04 parts by mass of cumene hydroperoxide (CHP) was continuously added to the glass reactor over a period of 120 minutes. After completion of the addition, 0.04 parts by mass of CHP was added to the glass reactor, and the mixture in the glass reactor was continuously stirred for an additional 2 hours to complete the polymerization. Through the above operations, an aqueous latex (L-1) containing polymer particles (component (C)) having a core-shell structure was obtained. The polymerization conversion rate of the monomer components was 99% or higher. The volume average particle diameter of the resulting polymer particles was 0.21 μm, and the epoxy group content relative to the total amount of the shell layer was 2.2 mmol / g.
[0168] 3. Preparation of Dispersion (M) in which Component (C) is Dispersed in Component (A) Production Example 3-1: Preparation of Dispersion (M-1) 132 g of methyl ethyl ketone (MEK) was introduced into a 1 L mixing tank at 25°C. Next, while stirring the MEK, 132 g of the aqueous latex (L-1) containing polymer particles obtained in Production Example 2-1 (containing 40 g of component (C)) was added to the mixing tank. After the raw materials in the mixing tank were uniformly mixed, 200 g of water was added to the mixing tank at a feed rate of 80 g / min while stirring the raw materials in the mixing tank. After the water supply was completed, the stirring was promptly stopped, and a slurry liquid consisting of aggregates containing component (C) and an aqueous phase containing a small amount of organic solvent was obtained. The aggregates were floatable. Next, 360 g of the aqueous phase was discharged from a discharge port at the bottom of the mixing tank, leaving a portion of the aggregates containing the aqueous phase in the mixing tank. 90 g of MEK was added to the obtained aggregates and mixed uniformly to obtain a dispersion in which the core-shell polymer was uniformly dispersed in MEK. 60 g of component (A-1) was added to the obtained dispersion and mixed uniformly. MEK was removed from the obtained mixture using a rotary evaporator. This operation yielded a dispersion (M-1) in which component (C) was dispersed in component (A-1).
[0169] (Curing accelerator (D)) Dyhard UR200 (manufactured by AlzChem, 3-(3,4-dichlorophenyl) (inorganic filler) Fumed silica: CAB-O-SIL TS-720 (manufactured by CABOT, fumed silica surface-treated with polydimethylsiloxane) Calcium carbonate: Whiten SB (manufactured by Shiraishi Calcium, untreated heavy calcium carbonate) Calcium oxide: CML#31 (manufactured by Omi Chemical Industry, calcium oxide surface-treated with fatty acid).
[0170] [Measurement Methods] The methods for measuring the various physical properties measured in the examples are shown below.
[0171] (Volume average particle diameter of polymer particles) The volume average particle diameter (Mv) of the polymer particles dispersed in the core-shell polymer latex described in the Production Examples was measured using a Microtrac UPA150 (manufactured by Nikkiso Co., Ltd.). In the measurement, a core-shell polymer latex diluted with deionized water was used as a measurement sample. The measurement was performed by inputting the refractive index of water and the refractive index of each polymer particle, adjusting the sample concentration so that the measurement time was 600 seconds, and the signal level was within the range of 0.6 to 0.8.
[0172] (Measurement of Glass Transition Temperature and Storage Modulus) The glass transition temperature and storage modulus of the cured product obtained by curing the curable resin composition were measured as follows: The curable resin composition was applied between two fluorine-coated steel plates measuring 25 mm wide and 100 mm long, and the two steel plates were overlapped so that the thickness of the curable resin composition was 0.2 to 1.3 mm. The cured product was then cured (low-temperature curing) at a curing temperature of 130°C for 20 minutes to obtain a laminate in which the two steel plates were bonded together by the cured product. The plate-shaped cured product was peeled from the obtained laminate, and its thickness was measured with a vernier caliper. Here, the thickness of the steel plate was the same as that used in the corresponding Examples or Comparative Examples (i.e., steel plates with thicknesses of 1.6 mm, 0.8 mm, or 0.5 mm). This cured product was cut into a strip of 30 mm length x 5 mm width, and the storage modulus E' at 23°C, 100°C, and 120°C, as well as the glass transition temperature (Tg1) in Celsius, which is the temperature at which the loss tangent (tanδ) becomes maximum, were measured using a dynamic mechanical analyzer (DMA) in tension mode at a frequency of 1 Hz.
[0173] (Glass transition temperature attainment rate) For each curable resin composition, the glass transition temperature (Tg2) of the cured product at the completion of the curing reaction was measured in Celsius using the same procedure as above, except that the curing conditions for the curable resin composition were changed to a curing temperature of 130°C and a curing time of 2 hours. The glass transition temperature attainment rate was calculated using the following formula: Glass transition temperature attainment rate = (Tg1 (°C) / Tg2 (°C)) × 100.
[0174] (Examples 1 to 7, Comparative Examples 1 to 4) Each component was weighed and thoroughly mixed to obtain the formulation shown in Table 1, thereby obtaining a curable resin composition. The curable resin composition was applied to a fluororesin-coated steel plate (first adherend) having a thickness shown in Table 1, and another fluororesin-coated steel plate (second adherend) having a thickness shown in Table 1 was then laminated to the first adherend (lamination step). The obtained structure was heat-cured (low-temperature curing) at a curing temperature of 130°C for a curing time of 20 minutes (curing step) to obtain a laminate. The physical properties of the obtained laminate (the cured product in the laminate) were measured and evaluated. The results are shown in Table 1.
[0175] According to one embodiment of the present invention, a method for producing a laminate can be provided in which adherends are bonded to each other by a cured product that has a high elastic modulus in a high-temperature environment even when cured at a low temperature for a short time. This production method can be suitably used for bonding steel plates, CFRP, aluminum plates, and concrete. Therefore, one embodiment of the present invention can be suitably used in the fields of vehicles, aircraft, space, machinery, electricity, architecture, and civil engineering.
Claims
1. A method for producing a laminate in which a first adherend, a cured product obtained by curing a curable resin composition, and a second adherend are laminated in this order, the method comprising: a step (i) of applying the curable resin composition to the first adherend and bonding the second adherend to the first adherend; and a step (ii) of curing the curable resin composition, the curable resin composition containing an epoxy resin (A) and 3.5 to 19.0 parts by mass of dicyandiamide (B) per 100 parts by mass of the epoxy resin (A), the epoxy resin (A) contains 51 to 100% by mass of unmodified bisphenol A type epoxy resin (A-1) relative to a total amount of 100% by mass of the epoxy resin (A), the curing temperature of the curable resin composition in the step (ii) is 105°C to 145°C, and the curing time of the curable resin composition in the step (ii) is 10 to 60 minutes, a ratio (Y / X) of a thickness (Y) of the cured product to an average thickness (X) of the first adherend and the second adherend is 0.5 to 10.
0.
2. The method for producing a laminate according to claim 1, wherein the glass transition temperature attainment rate of the cured product is 80% or more; wherein the glass transition temperature attainment rate of the cured product is a value calculated by the following formula: glass transition temperature attainment rate of the cured product=(glass transition temperature (Tg1) (°C) in Celsius of the cured product obtained by curing the curable resin composition at a curing temperature of 130°C for a curing time of 20 minutes / glass transition temperature (Tg2) (°C) in Celsius of the cured product obtained by curing the curable resin composition under conditions of a curing temperature of 130°C for a curing time of 120 minutes)×100.
3. A method for producing a laminate according to claim 1, wherein the storage modulus of the cured product at 23°C is 1 GPa or more, and the storage modulus is a value obtained by measuring at a frequency of 1 Hz using a tensile mode of dynamic viscoelasticity measurement.
4. A method for producing a laminate as described in claim 1, wherein the storage modulus of the cured product at 120°C is 0.07 GPa or more, and the storage modulus is a value obtained by measuring at a frequency of 1 Hz using a tensile mode of dynamic viscoelasticity measurement.
5. The method for producing a laminate according to claim 2, wherein the glass transition temperature (Tg1) of the cured product is 120°C or higher.
6. The method for producing a laminate according to claim 1, wherein the epoxy resin (A) does not contain an aliphatic polybasic acid-modified epoxy resin (A-3).
7. The method for producing a laminate according to claim 1, wherein the epoxy resin (A) contains an aliphatic polybasic acid-modified epoxy resin (A-3), and the content of the aliphatic polybasic acid-modified epoxy resin (A-3) in the epoxy resin is greater than 0 mass% and less than 3 mass%.
8. The method for producing a laminate according to claim 1, wherein the first adherend and / or the second adherend is a steel plate.
9. The method for producing a laminate according to claim 1, wherein the curable resin composition further contains 1 to 100 parts by mass of polymer particles (C) having a core-shell structure including a core layer and a shell layer, relative to 100 parts by mass of the epoxy resin (A).
10. The method for producing a laminate according to claim 1, wherein the curable resin composition further contains 0.1 to 15 parts by mass of a curing accelerator (D) per 100 parts by mass of the epoxy resin (A).
11. The method for producing a laminate according to claim 9, wherein the core layer comprises at least one rubber selected from the group consisting of diene rubber, (meth)acrylate rubber, and organosiloxane rubber.
12. The method for producing a laminate according to claim 9, wherein the core layer is butadiene rubber and / or butadiene / styrene rubber.
13. The method for producing a laminate according to claim 9, wherein the shell layer contains structural units derived from one or more monomers selected from the group consisting of aromatic vinyl monomers, vinylcyan monomers, and (meth)acrylate monomers.
14. A method for manufacturing a vehicle body structure, comprising a method for manufacturing a laminate according to any one of claims 1 to 13.
Citation Information
Patent Citations
Epoxy adhesive composition for electric-powered steering device, bonded structure and electric-powered steering device
JP2005015563A
One-pack type epoxy resin-based adhesive
JP2011148867A
Structural adhesives and their application to bonding
JP2015501853A
Epoxy resin composition
JP2023032370A
Laminated body and production method therefor, and automotive exterior material