Polyamide resin composition, film and film laminate comprising same, and pellet mixture
The polyamide resin composition addresses the recyclability and physical property issues in packaging materials by combining aliphatic polyamides, ethylene/α-olefin copolymers, and antioxidants, resulting in transparent, strong films with pinhole resistance and improved recyclability.
Patent Information
- Application Number
- PCT/JP2024/009054
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-08
- Publication Date
- 2024-10-03
AI Technical Summary
Current polyamide resin compositions for packaging materials, such as food packaging, face challenges in recyclability due to poor compatibility between different resin types, leading to deteriorated physical properties and limited reuse potential, despite containing compatibilizers like modified ethylene/α-olefin copolymers, which can cause film gel and reduce transparency.
A polyamide resin composition comprising 88-99% aliphatic polyamide resin, 1-50% aliphatic homopolyamide or copolyamide, and 1-5% ethylene/α-olefin copolymer with specific functional groups, along with optional antioxidants and polyolefins, optimized to maintain transparency, mechanical strength, and prevent film gel, while enabling effective recycling by improving layer compatibility.
The composition achieves transparent, mechanically strong films with pinhole resistance and prevents film gel, allowing for efficient recycling of laminated films by enhancing compatibility between polyamide and polyolefin layers, thus improving material recyclability.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Polyamide resin composition, film and film laminate containing the same, and pellet mixture
[0001] The present invention relates to a polyamide resin composition, a film and a film laminate containing the same, and a pellet mixture.
[0002] In recent years, the recycling of plastic waste has become increasingly desirable due to issues such as global warming and marine pollution. Packaging materials, such as food packaging, are often laminates made of different resins, such as polyamides and polyolefins, to provide functionality. While separating these waste materials by delamination is considered a viable approach, it is technically difficult and unrealistic. On the other hand, if the laminate is recycled without delamination, the poor compatibility of the different resins results in significantly reduced physical properties of the recycled mixed resin, limiting its applications. To achieve good blending of different resins, a compatibilizer can be used. Modified ethylene / α-olefin copolymers are known as compatibilizers for polyamides and polyolefins. Furthermore, polyamide resin compositions must maintain the physical properties of the films obtained from these compositions before recycling while improving their material recyclability. For packaging materials such as food packaging, polyamide resin compositions are required to have high transparency, tensile strength, puncture resistance, pinhole resistance, and minimal film gel. Depending on the application, flexibility and stretchability are also required, and it is known to use aliphatic copolyamides to impart flexibility and stretchability to polyamide films.
[0003] Patent Document 1 discloses a multilayer structure of a nylon-containing polar layer and a polyolefin layer, in which the polyolefin layer contains a compatibilizer component containing an anhydride and / or carboxylic acid-functionalized ethylene / α-olefin interpolymer having a specific melt viscosity and density, and indicates that waste multilayer structures can be recycled. Patent Document 2 discloses a laminate having a layer configuration having a sealant layer and a reinforcing layer, in which the sealant layer contains a linear low-density polyethylene and a compatibilizer that is an unsaturated carboxylic acid-modified polyolefin, and the reinforcing layer contains a polyamide resin, thereby improving recyclability.
[0004] Patent Document 3 describes a method for producing a polyester film containing 100 parts by mass of polyamide (A) and a density of 0.915 to 0.975 g / cm 3 Patent Document 4 discloses a polyamide resin composition containing 3 to 30 parts by mass of an acid-modified polyethylene (E), and indicates that the composition has excellent heat aging resistance and is suitable for use in automotive parts. Patent Document 4 discloses a polyamide resin blend comprising (A) a masterbatch obtained by melt-mixing (a) a polyamide resin and a modified ethylene-α-olefin copolymer in a weight ratio of 40 / 60 to 99 / 1, and (B) a polyamide resin in a weight ratio of 1 / 99 to 60 / 40, and indicates that a polyamide film molded from the blend has excellent pinhole resistance and transparency and little occurrence of fisheyes. In the examples of Patent Documents 3 and 4, only polyamide 6 is used as the polyamide resin.
[0005] Patent Document 5 discloses a polyamide resin composition containing (A) a linear aliphatic nylon copolymer having a melting point of 130°C or less and (B) a modified polyolefin resin in a specified ratio, and demonstrates that a nylon laminate with excellent thermal adhesiveness can be obtained by simple and inexpensive coextrusion molding. Patent Document 6 discloses a polyamide resin composition containing a polyamide resin (A) including an aliphatic homopolyamide and a copolymerized polyamide, and an impact-resistant material (B) such as a maleic anhydride-modified ethylene-butene copolymer in a specified ratio, and demonstrates that the composition exhibits excellent blow moldability while maintaining a good surface appearance of the molded article. Patent Document 7 discloses a hydrogen tank liner material composed of a polyamide resin composition containing (A) polyamide 6, (B) a copolymerized polyamide, and (C) an impact-resistant material in a specified ratio, and demonstrates that the material has excellent gas barrier properties and impact resistance at cryogenic temperatures. Patent Document 8 discloses a polyamide resin composition containing a polyamide resin and a modified polyolefin resin in a specified ratio, and demonstrates that the composition has excellent heat resistance and is suitable for producing blow-molded products.
[0006] Furthermore, Patent Document 9 discloses a pelletizable thermoplastic polymer composition comprising (a) a polyamide and (b) a polymer polymerized from maleic anhydride and an olefin, and indicates that it is possible to obtain a product with improved durability, etc. Patent Document 10 discloses a masterbatch composition for use in preparing a polyamide blend from a polyamide, which comprises an olefin-maleic anhydride copolymer and one or more carrier resins, and indicates that the masterbatch composition has good compatibility and does not cause phase separation, etc.
[0007] Japanese Patent Publication No. 2018-502743 Japanese Patent Publication No. 2020-11415 Japanese Patent Publication No. 2019-38938 Japanese Patent Publication No. 2000-109685 Japanese Patent Publication No. 7-3109 Japanese Patent Publication No. 2017-206639 Japanese Patent Publication No. 2009-191871 Japanese Patent Publication No. 4-239559 Japanese Patent Publication No. 2014-503003 Japanese Patent Publication No. 2015-525813
[0008] It is thought that the inclusion of a compatibilizer in a laminate can improve the recyclability of the laminate waste. Patent Documents 1 and 2 only disclose the inclusion of a compatibilizer in a polyolefin layer, but do not disclose the inclusion of a compatibilizer in a polyamide layer. In general, when a compatibilizer such as a modified polyolefin is added to a polyamide, problems such as the generation of film gel and a decrease in transparency occur.
[0009] The polyamide resin compositions of Patent Documents 3 to 10 contain a polyamide resin and a modified polyolefin resin in a predetermined ratio, but these compositions are intended to improve properties such as heat aging resistance, transparency, moldability, impact resistance, and thermal adhesiveness, and do not take into consideration the recyclability of waste molded articles obtained, resulting in insufficient recyclability.
[0010] Furthermore, the polyamide resin compositions of Patent Documents 3, 5, 7, and 8 are intended for use in automobile parts, laminates with nonwoven fabrics, woven fabrics, etc., and are difficult to apply to packaging materials such as food packaging, where problems such as the generation of film gels and reduced transparency arise. Films obtained from the polyamide resin blend of Patent Document 4 exhibit certain pinhole resistance, transparency, reduced film gels, etc., but the levels are insufficient. Films obtained from the compositions of Patent Documents 6, 9, and 10 have insufficient physical properties such as film gels.
[0011] The present invention aims to provide a polyamide resin composition that provides a film that is free from deterioration in appearance due to film gel and has excellent transparency, mechanical strength, and pinhole resistance, and that enables material recycling of laminates of the film with films of different resins, as well as a film and a film laminate using the same. Another object of the present invention is to provide a pellet mixture that is suitable for use in producing the polyamide resin composition, film, and film laminate.
[0012] The present invention relates to the following items [1] to
[19] . [1] A polyamide resin composition containing, relative to 100% by mass of the polyamide resin composition, 88 to 99% by mass of an aliphatic polyamide resin (A), 1 to 5% by mass of an ethylene / α-olefin copolymer having 3 to 8 carbon atoms having a functional group (B), and 0 to 9% by mass of another component (C); in the aliphatic polyamide resin (A), the ratio of the number of methylene groups to the number of amide groups is 3 or more and 11 or less; and the aliphatic polyamide resin (A) is [2] A polyamide resin composition according to [1], wherein the DSC curve obtained by heating the polyamide resin composition from 0°C to 280°C at a rate of 20°C / min in an air atmosphere has a melting peak in the range of 150 to 205°C, and the number average molecular weight Mn of the polyamide resin composition measured by GPC is 50,000 to 60,000. [3] The polyamide resin composition according to [1] or [2], wherein the aliphatic copolyamide (A-2) is a copolymer selected from the group consisting of polyamide 6 / 66, polyamide 6 / 69, polyamide 6 / 11, polyamide 6 / 12, polyamide 6 / 66 / 11, and polyamide 6 / 66 / 12. [4] The polyamide resin composition according to any one of [1] to [3], wherein the copolymer (B) is an ethylene / propylene copolymer, ethylene / 1-butene copolymer, ethylene / 1-hexene copolymer, or ethylene / 1-octene copolymer having a group derived from maleic anhydride. [5] The polyamide resin composition according to any one of [1] to [4], wherein the other component (C) comprises a polyolefin (D) having no functional group, and the content of the component (D) relative to 100% by mass of the polyamide resin composition is 2 to 8% by mass. [6] The polyamide resin composition according to any one of [1] to [5], wherein the other component (C) includes an antioxidant, and the content of the antioxidant relative to 100% by mass of the polyamide resin composition is 0.01 to 1% by mass.[7] The polyamide resin composition according to any one of [1] to [6], wherein the other component (C) comprises compound (E) selected from the group consisting of methylene bis-stearamide, ethylene bis-stearamide, butylene bis-stearamide, and hexamethylene bis-stearamide, and the content of compound (E) is 0.01 to 1 mass% based on 100 mass% of the polyamide resin composition. [8] The polyamide resin composition according to any one of [1] to [7], wherein the other component (C) comprises compound (F) selected from the group consisting of terminal-modified polyalkylene glycols, phosphate esters or phosphites, higher fatty acid monoesters, higher fatty acids, metal salts of higher fatty acids, higher fatty acid monoamides, N-substituted higher fatty acid monoamides, magnesium silicate, and substituted benzylidene sorbitols, and the content of compound (F) is 0.01 to 1 mass% based on 100 mass% of the polyamide resin composition. [9] The polyamide resin composition according to any one of [1] to [8], which is substantially free of silica.
[10] A polyamide film comprising the polyamide resin composition according to any one of [1] to [9].
[11] A laminate film comprising at least three layers, in which a layer comprising the polyamide resin composition according to any one of [1] to [9], an adhesive layer, and a polyolefin layer are laminated in this order.
[12] A laminate film comprising at least five layers, in which an adhesive layer and a polyolefin layer are laminated, in this order, on both sides of a layer comprising the polyamide resin composition according to any one of [1] to [9].
[13] The laminate film according to
[11] or
[12] , wherein the layer comprising the polyamide resin composition is a biaxially stretched layer.
[14] The laminate film according to any one of
[11] to
[13] , which is used for food packaging.
[15] A pellet mixture comprising: first pellets containing a first aliphatic polyamide resin (a1) and a functional group-containing ethylene / C3-C8 α-olefin copolymer (B); and second pellets containing a second aliphatic polyamide resin (a2), the first pellets (100% by mass) contain 60 to 90% by mass of a first aliphatic polyamide resin (a1), 10 to 40% by mass of the copolymer (B), and 0 to 9% by mass of another component (C), and the aliphatic polyamide resin (a1) is an aliphatic homopolyamide; the second aliphatic polyamide resin (a2) contains 0 to 20% by mass of an aliphatic homopolyamide and 80 to 100% by mass of an aliphatic copolyamide, relative to 100% by mass of the aliphatic polyamide resin (a2); the content of the aliphatic homopolyamide is 1 to 50% by mass, and the content of the aliphatic copolyamide is 50 to 99% by mass, relative to 100% by mass of the total of the first aliphatic polyamide resin (a1) and the second aliphatic polyamide resin (a2); in the aliphatic polyamide resin (a1) and the aliphatic polyamide resin (a2), the ratio of the number of methylene groups to the number of amide groups is 3 or more and 11 or less,
[16] The pellet mixture according to
[15] , further comprising a third pellet containing a polyolefin (D) having no functional groups, wherein the content of the component (D) is 2 to 8% by mass.
[17] The pellet mixture according to
[15] or
[16] , further comprising a third pellet containing a polyolefin (D) having no functional groups, wherein the content of the component (D) is 2 to 8% by mass relative to 100% by mass of the melt-kneaded mixture.
[18] The pellet mixture according to
[15] or
[16] , further comprising a third pellet containing a polyolefin (D) having no functional groups, wherein the content of the component (D) relative to 100% by mass of the melt-kneaded mixture is 2 to 8% by mass.
[19] The pellet mixture according to
[18] or
[19] , further comprising a third pellet containing a polyolefin (D) having no functional groups, wherein the content of the component (D) relative to 100% by mass of the melt-kneaded mixture is 2 to 8% by mass.
[20] The pellet mixture according to
[18] or
[20] , further comprising a third pellet containing a polyolefin (D) having no functional groups, wherein the content of the component (D) relative to 100% by mass of the melt-kneaded mixture is 2 to 8% by mass.
[21] The pellet mixture according to
[18] or
[19] , further comprising a third pellet containing a polyolefin (D) having no functional groups, wherein the content of the component (D) relative to 100% by mass of the melt-kneaded mixture is 2 to 8% by mass.
[22] The pellet mixture according to
[18] or
[19] , further comprising a third pellet containing a polyolefin (D) having no functional groups, wherein the content of the component (D) relative to 100% by mass of the melt-kneaded mixture is 2 to 8% by mass.
[23] The pellet mixture according to
[18] or
[19] , further comprising a third
[18] The first pellets to be mixed with the second pellets in the production of the pellet mixture according to any one of
[15] to
[17] .
[19] The second pellets to be mixed with the first pellets in the production of the pellet mixture according to any one of
[15] to
[17] .
[0013] According to the present invention, there are provided a polyamide resin composition that provides a film that is free from deterioration in appearance due to film gel and that is excellent in transparency, mechanical strength, and pinhole resistance, and that enables material recycling of a laminate of the film with a different resin film, as well as a film and a film laminate using the same.Furthermore, there is provided a pellet mixture that is suitably used for producing the polyamide resin composition, film, and film laminate.
[0014] In this specification, the content of each component in a composition refers to the total amount of the components when the composition contains multiple substances corresponding to each component, unless otherwise specified. In this specification, the term "polyamide resin composition" refers to a composition containing at least a polyamide resin, and includes any form such as pellets, sheets, strands, chips, and molded products formed by various methods. The term "pellets" refers to one of the forms that a polyamide resin composition can take. The polyamide resin composition and pellets according to the present invention will be described in detail below.
[0015] The polyamide resin composition of the present invention contains, relative to 100% by mass of the polyamide resin composition, 88 to 99% by mass of an aliphatic polyamide resin (A), 1 to 5% by mass of a functional group-containing ethylene / α-olefin copolymer (B) having 3 to 8 carbon atoms, and 0 to 9% by mass of another component (C); in the aliphatic polyamide resin (A), the ratio of the number of methylene groups to the number of amide groups is 3 or more and 11 or less; the aliphatic polyamide resin (A) contains, relative to 100% by mass of the aliphatic polyamide resin (A), 1 to 50% by mass of an aliphatic homopolyamide (A-1) and 50 to 99% by mass of an aliphatic copolyamide (A-2); the polyamide resin composition has a melting peak in the range of 150 to 205°C in a DSC curve obtained by heating the polyamide resin composition from 0°C to 280°C at a rate of 20°C / min in an air atmosphere; and the polyamide resin composition has a number average molecular weight Mn of 50,000 to 60,000 as measured by GPC. By using the polyamide resin composition of the present invention, it is possible to obtain a film that is free from deterioration in appearance due to film gel and that has excellent transparency, mechanical strength such as tensile strength, elongation, and puncture resistance, and pinhole resistance, and it also becomes possible to materially recycle film waste.
[0016] In the present invention, material recycling means reusing waste as a raw material for a product. Specifically, it means processing a laminate film including a layer containing a polyamide resin composition, particularly a laminate film including at least a layer containing a polyamide resin composition and a layer containing a polyolefin, such as by cutting and pulverizing the waste, melt-kneading the resulting material, and forming it into pellets or the like, and then reusing the resulting material as a raw material for a new plastic product.
[0017] [Polyamide Resin Composition] <Aliphatic Polyamide Resin (A)> The aliphatic polyamide resin (A) contains an aliphatic group in a constituent repeating unit and has an amide bond (—CONH—) in the main chain. Examples of the aliphatic polyamide resin (A) include aliphatic homopolyamides and aliphatic copolyamides, and these may be used alone or in combination of two or more.
[0018] (Aliphatic homopolyamide (A-1)) The aliphatic homopolyamide (A-1) is a polyamide resin composed of one type of structural unit derived from an aliphatic monomer. The aliphatic homopolyamide (A-1) may be composed of at least one type of lactam and an aminocarboxylic acid that is a hydrolyzate of the lactam, or may be composed of a combination of one type of diamine and one type of dicarboxylic acid. Here, the combination of one type of diamine and one type of dicarboxylic acid is considered to be one type of monomer.
[0019] Examples of lactams include ε-caprolactam, enantholactam, undecane lactam, dodecane lactam (ω-laurolactam), α-pyrrolidone, and α-piperidone. Among these, from the viewpoint of polymerization productivity, one selected from the group consisting of ε-caprolactam, undecane lactam, and dodecane lactam is preferred. Examples of aminocarboxylic acids include ε-aminocaproic acid, 7-aminoheptanoic acid, 9-aminononanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid.
[0020] Examples of diamines include aliphatic diamines such as ethylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, tridecanediamine, tetradecanediamine, pentadecanediamine, hexadecanediamine, heptadecanediamine, octadecanediamine, nonadecanediamine, eicosanediamine, 2-methyl-1,8-octanediamine, and 2,2,4 / 2,4,4-trimethylhexamethylenediamine.
[0021] Examples of dicarboxylic acids include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedionic acid, dodecanedionic acid, tridecanedionic acid, tetradecanedionic acid, pentadecanedioic acid, hexadecanedioic acid, octadecanedioic acid, and eicosanedioic acid.
[0022] Specific examples of the aliphatic homopolyamide (A-1) include polyamide 4, polyamide 6, polyamide 7, polyamide 9, polyamide 10, polyamide 11, polyamide 12, polyamide 26, polyamide 44, polyamide 45, polyamide 46, polyamide 48, polyamide 49, polyamide 54, polyamide 55, polyamide 56, polyamide 66, polyamide 410, polyamide 412, polyamide 58, polyamide 59, polyamide 510, polyamide 512, polyamide 64, and polyamide 6. Examples of the aliphatic homopolyamide (A-1) include polyamide 5, polyamide 68, polyamide 69, polyamide 610, polyamide 611, polyamide 612, polyamide 96, polyamide 98, polyamide 99, polyamide 105, polyamide 616, polyamide 618, polyamide 910, polyamide 912, polyamide 106, polyamide 108, polyamide 109, polyamide 1010, polyamide 1012, polyamide 125, polyamide 126, polyamide 129, polyamide 1210, polyamide 1212, and polyamide 122. These aliphatic homopolyamides (A-1) can be used alone or as a mixture of two or more. Among these, polyamide 6 or polyamide 66 is preferred, with polyamide 6 being particularly preferred, from the viewpoints of availability, economy, and the mechanical properties and heat resistance of the resulting molded article.
[0023] (Aliphatic Copolyamide (A-2)) The aliphatic copolyamide (A-2) is a polyamide resin composed of two or more structural units derived from aliphatic monomers. The structural units of the aliphatic copolyamide (A-2) are derived from a monomer selected from the group consisting of a combination of a diamine and a dicarboxylic acid, a lactam, and an aminocarboxylic acid. Here, a combination of a diamine and a dicarboxylic acid is considered to be one type of monomer, with one type of diamine and one type of dicarboxylic acid being the combination.
[0024] Examples of diamines include the same as those exemplified as raw materials for the aliphatic homopolyamide (A-1).
[0025] Examples of dicarboxylic acids include the same as those exemplified as raw materials for the aliphatic homopolyamide (A-1).
[0026] Examples of lactams include those exemplified as raw materials for the aliphatic homopolyamide (A-1). Examples of aminocarboxylic acids include those exemplified as raw materials for the aliphatic homopolyamide (A-1). These diamines, dicarboxylic acids, lactams, and aminocarboxylic acids may be used alone or in combination of two or more.
[0027] Specific examples of the aliphatic copolyamide (A-2) include copolymers combining two or more of the monomers forming the polyamides exemplified as the aliphatic homopolyamide (A-1), more specifically, aliphatic copolyamides such as polyamide 4 / 6, polyamide 6 / 66, polyamide 6 / 69, polyamide 6 / 610, polyamide 6 / 611, polyamide 6 / 612, polyamide 6 / 10, polyamide 6 / 11, polyamide 6 / 12, polyamide 6 / 66 / 11, polyamide 6 / 66 / 12, polyamide 6 / 66 / 610, polyamide 6 / 66 / 612, polyamide 6 / 610 / 12 and polyamide 6 / 612 / 12. These aliphatic copolyamides (A-2) can be used alone or as a mixture of two or more.
[0028] From the viewpoints of transparency, flexibility, and stretchability, the aliphatic copolyamide (A-2) is preferably selected from the group consisting of polyamide 6 / 66, polyamide 6 / 69, polyamide 6 / 11, polyamide 6 / 12, polyamide 6 / 66 / 11, polyamide 6 / 66 / 12, polyamide 6 / 610 / 12, and polyamide 6 / 612 / 12, more preferably selected from the group consisting of polyamide 6 / 66, polyamide 6 / 69, polyamide 6 / 11, polyamide 6 / 12, polyamide 6 / 66 / 11, and polyamide 6 / 66 / 12, even more preferably selected from the group consisting of polyamide 6 / 66, polyamide 6 / 12, and polyamide 6 / 66 / 12, with polyamide 6 / 66 being particularly preferred. From the viewpoints of transparency, flexibility, and stretchability, the copolymerization ratio of polyamide 6 in these aliphatic copolyamides (A-2) is preferably 50% by mass or more, more preferably 70 to 95% by mass, and even more preferably 75 to 90% by mass.
[0029] (Method for producing aliphatic polyamide resin (A)) Examples of an apparatus for producing aliphatic polyamide resin (A) include known polyamide production apparatuses such as batch-type reaction vessels, single- or multi-vessel continuous reaction vessels, tubular continuous reaction vessels, kneading reaction extruders such as single-screw kneading extruders and twin-screw kneading extruders. As the polymerization method, known methods such as melt polymerization, solution polymerization, and solid-phase polymerization can be used, and polymerization can be carried out by repeating operations such as normal pressure, reduced pressure, and increased pressure. These polymerization methods can be used alone or in appropriate combination.
[0030] (Ratio of the number of methylene groups to the number of amide groups) In the aliphatic polyamide resin (A), the ratio of the number of methylene groups ([CH 2 ]) to the number of amide groups ([NHCO]) [CH 2 ] / [NHCO] (hereinafter, the ratio of the number of methylene groups to the number of amide groups is referred to as [CH 2 ] / [NHCO]. ) is 3 or more and 11 or less. [CH 2 By setting [CH ] / [NHCO] within the above range, it is possible to improve the molding processability, and the mechanical properties and heat resistance of the obtained molded article. 2] / [NHCO] is preferably 3 or more and 9 or less, more preferably 4 or more and 8 or less, and even more preferably 4 or more and 7 or less.
[0031] The ratio of the number of methylene groups to the number of amide groups [CH 2 Examples of aliphatic homopolyamides having a ratio of ] / [NHCO] of 3 to 11 include polyamide 4:3.0, polyamide 6:5.0, polyamide 7:6.0, polyamide 9:8.0, polyamide 10:9.0, polyamide 11:10.0, polyamide 12:11.0, polyamide 26:3.0, polyamide 44:3.0, polyamide 45:3.5, polyamide 46:4.0, polyamide 48:5.0, polyamide 49:5.5, polyamide 410:6.0, polyamide 412:7.0, polyamide 54:3.5, polyamide 55:4.0, polyamide 56:4.5, polyamide 58:5.5, polyamide 59:6.0, polyamide 510:6.5, polyamide 512:7.5, polyamide 64:4.0, and polyamide 65:4. 5, Polyamide 66:5.0, Polyamide 68:6.0, Polyamide 69:6.5, Polyamide 610:7.0, Polyamide 611:7.5, Polyamide 612:8.0, Polyamide 616:10.0, Polyamide 618:11.0, Polyamide 96:6.5, Polyamide 98:7.5, Polyamide 99:8.0, Polyamide 910:8.5, Polyamide 912 :9.5, polyamide 105:6.5, polyamide 106:7.0, polyamide 108:8.0, polyamide 109:8.5, polyamide 1010:9.0, polyamide 1012:10.0, polyamide 125:7.5, polyamide 126:8.0, polyamide 129:9.5, polyamide 1210:10.0, polyamide 1212:11.0, etc. In addition, the ratio of the number of methylene groups to the number of amide groups [CH 2 Examples of the aliphatic copolyamide having a [N-HCO] / [NHCO] ratio of 3 to 11 include copolymers using several raw material monomers that form the aliphatic homopolyamide. These may be used alone or in combination of two or more.
[0032] In the case of the aliphatic copolyamide (A-2), the ratio of the number of methylene groups to the number of amide groups [CH 2] / [NHCO] is the ratio of the number of methylene groups to the number of amide groups in the homopolymer of the monomer constituting the repeating unit of the copolymer [CH 2 ] / [NHCO] by the mole fraction of the constituent repeating unit, and the resulting values can be added up for all the constituent repeating units.
[0033] When the aliphatic polyamide resin (A) is a mixture of two or more aliphatic polyamide resins, the ratio of the number of methylene groups to the number of amide groups [CH 2 ] / [NHCO] is the ratio of the number of methylene groups to the number of amide groups in each aliphatic polyamide resin [CH 2 ] / [NHCO] by the mixing ratio expressed as a molar ratio, and then adding up the values obtained for all the aliphatic polyamide resins.
[0034] (Contents of Aliphatic Homopolyamide (A-1) and Aliphatic Copolymer Polyamide (A-2)) The aliphatic polyamide resin (A) contains 1 to 50 mass% of aliphatic homopolyamide (A-1) and 50 to 99 mass% of aliphatic copolymer polyamide (A-2) relative to 100 mass% of the aliphatic polyamide resin (A). By setting the contents of the aliphatic homopolyamide (A-1) and the aliphatic copolymer polyamide (A-2) within the above ranges, transparency, flexibility, and stretchability can be improved. If the content of the aliphatic homopolyamide (A-1) is less than 1 mass%, the transparency of the film formed is deteriorated, and if it exceeds 50 mass%, the flexibility and stretchability are deteriorated. If the content of the aliphatic copolymer polyamide (A-2) is less than 50 mass%, the flexibility and stretchability are deteriorated, and if it exceeds 99 mass%, the transparency and coefficient of friction of the film formed is deteriorated. The content of the aliphatic homopolyamide (A-1) relative to 100% by mass of the aliphatic polyamide resin (A) is preferably 3 to 30% by mass, more preferably 4 to 20% by mass, and particularly preferably 5 to 15% by mass. The content of the aliphatic copolyamide (A-2) relative to 100% by mass of the aliphatic polyamide resin (A) is preferably 70 to 97% by mass, more preferably 80 to 96% by mass, and particularly preferably 85 to 95% by mass.
[0035] (Preferred Aspects of Aliphatic Homopolyamide (A-1) and Aliphatic Copolyamide (A-2)) From the viewpoints of reducing film gel when formed into a film and improving transparency, puncture strength, and pinhole resistance, the aliphatic homopolyamide (A-1) is preferably polyamide 6, and the aliphatic copolyamide (A-2) is preferably selected from the group consisting of polyamide 6 / 66, polyamide 6 / 69, polyamide 6 / 11, polyamide 6 / 12, polyamide 6 / 66 / 11, and polyamide 6 / 66 / 12. Of these, a combination in which the aliphatic homopolyamide (A-1) is polyamide 6 and the aliphatic copolyamide (A-2) is polyamide 6 / 66 is particularly preferred.
[0036] (Physical Properties of Aliphatic Polyamide Resin (A)) From the viewpoint of moldability, the relative viscosity of the aliphatic polyamide resin (A) is preferably 2.0 to 5.0, more preferably 2.0 to 4.5, and even more preferably 2.1 to 4.0. By setting the relative viscosity of the aliphatic polyamide resin (A) within the above range, it becomes easier to ensure the moldability of the film and the mechanical strength of the obtained film.
[0037] The relative viscosity of the aliphatic polyamide resin (A) is a value measured at 25°C by dissolving 1 g of the polyamide resin (A) in 100 ml of 96% sulfuric acid in accordance with JIS K 6920. When the aliphatic polyamide resin (A) is a combination of two or more types, it is preferable to measure the relative viscosity by the above-mentioned method, but when the relative viscosity of each polyamide resin and its mixing ratio are known, the average value calculated by multiplying each relative viscosity by the mixing ratio may be used as the relative viscosity of the aliphatic polyamide resin (A).
[0038] From the viewpoint of improving the material recyclability of film waste, the melting point of the aliphatic polyamide resin (A) is preferably 150 to 205°C, more preferably 150 to 200°C, and even more preferably 160 to 198°C. The melting point of the aliphatic polyamide resin (A) refers to the melting point of the mixture of the aliphatic homopolyamide (A-1) and the aliphatic copolymer polyamide (A-2) constituting the polyamide resin composition. If the melting point of the aliphatic polyamide resin (A) is less than 150°C, the mechanical strength of the molded product deteriorates. If the melting point of the aliphatic polyamide resin (A) exceeds 205°C, material recyclability deteriorates. Specifically, for a laminate film containing at least a layer containing a polyamide resin composition and a layer containing a polyolefin, if the melting point exceeds 205°C, excessive heating is required when the waste is melt-kneaded and processed into pellets, etc., resulting in discoloration and thermal degradation of the polyolefin contained in the waste. The melting point is the melting peak temperature in a DSC curve obtained by heating an aliphatic polyamide resin (A) to 280°C in an air atmosphere, maintaining the temperature at that temperature for 5 minutes, then lowering the temperature to 0°C at a rate of 20°C / min, and then heating from 0°C to 280°C at a rate of 20°C / min.
[0039] From the viewpoint of reducing film gel, the terminal amino group concentration of the aliphatic polyamide resin (A) is 2.0 to 5.5 × 10 -5 eq / g, and preferably 2.5 to 5.0 × 10 -5 eq / g, more preferably 2.8 to 4.8 × 10 -5 The terminal amino group concentration can be expressed as the equivalent of amino groups per 1 g of polymer, and can be measured by dissolving the polyamide resin in a phenol / methanol mixed solution and titrating with 1 / 50 N hydrochloric acid.
[0040] When the aliphatic polyamide resin (A) contains two or more polyamide resin components having different terminal amino group concentrations, the terminal amino group concentration in the polyamide resin is preferably measured by the neutralization titration method described above. However, when the terminal amino group concentration of each polyamide resin component and its mixing ratio are known, the terminal amino group concentration of the polyamide resin may be determined by adding up the values obtained by multiplying each terminal amino group concentration by the mixing ratio. The terminal amino group concentration of the polyamide resin may be determined by averaging the total values.
[0041] From the viewpoints of suppressing the occurrence of film gels and improving the mechanical properties of polyamide films molded from the polyamide resin composition, the number-average molecular weight Mn of the aliphatic polyamide resin (A) as measured by GPC is preferably 50,000 to 60,000, more preferably 53,000 to 60,000, and even more preferably 55,000 to 60,000. Furthermore, the ratio of the weight-average molecular weight Mw to the number-average molecular weight Mn of the aliphatic polyamide resin (A) as measured by GPC, Mw / Mn, is preferably 1.5 to 3.0, more preferably 1.5 to 2.8, and even more preferably 1.6 to 2.5. The Mn and Mw values are measured by gel permeation chromatography (GPC).
[0042] From the viewpoint of moldability, the aliphatic polyamide resin (A) preferably has a melt flow rate (MFR) measured in accordance with ASTM D1238 at 230°C under a load of 2.16 kg of 1 to 100 g / 10 min, more preferably 2 to 90 g / 10 min, and even more preferably 3 to 80 g / 10 min.
[0043] (Aliphatic Polyamide Resin (A) Content) The content of the aliphatic polyamide resin (A) is 88 to 99% by mass based on 100% by mass of the polyamide resin composition. By setting the content of the aliphatic polyamide resin (A) within this range, the aliphatic polyamide resin (A) and the functional group-containing ethylene / α-olefin copolymer (B) having 3 to 8 carbon atoms exhibit good compatibility, improving the melt stability of the polyamide resin composition and the formability of the film. Furthermore, deterioration of the appearance of a polyamide film formed from the polyamide resin composition due to film gel can be suppressed, and the transparency and good pinhole resistance of the film can be maintained. Furthermore, the material recyclability of the film waste is also improved. The content of the aliphatic polyamide resin (A) is preferably 89 to 98% by mass based on 100% by mass of the polyamide resin composition.
[0044] <Functional Group-Containing Ethylene / C3-8 α-Olefin Copolymer (B) (Hereinafter, also referred to as Copolymer (B))> The polyamide resin composition contains a functional group-containing ethylene / C3-8 α-olefin copolymer (B). The inclusion of copolymer (B) can improve the pinhole resistance of films molded from the polyamide resin composition in low-temperature environments. Furthermore, due to the presence of a functional group, copolymer (B) functions as a compatibilizer between polyamide and polyolefin. Therefore, when a laminate film containing at least a layer containing a polyamide resin composition and a layer containing a polyolefin is recycled from waste film, the compatibility between the two layers is improved, resulting in improved homogeneity of the recycled plastic raw material. Copolymer (B) may be one type or a combination of two or more types.
[0045] Examples of functional groups in the copolymer (B) include a carboxyl group (which may be in the form of a salt), an acid anhydride group, a carboxylic acid ester group, a carboxylic acid imide group, a carboxylic acid amide group, and an epoxy group. It is believed that at least a portion of the amino groups in the aliphatic polyamide resin (A) react with these functional groups. Among these, from the viewpoint of compatibility between the polyamide and the polyolefin, at least one selected from the group consisting of a carboxyl group, a carboxylic acid ester group, and an acid anhydride group is preferred, and an acid anhydride group is more preferred.
[0046] Methods for introducing a functional group into an ethylene / C3-8 α-olefin copolymer include (i) copolymerizing a copolymerizable monomer having a functional group during copolymerization of the copolymer, (ii) introducing a functional group into the molecular chain or molecular end of the ethylene / C3-8 α-olefin copolymer using a polymerization initiator, chain transfer agent, or the like, and (iii) grafting a compound having the functional group and a graftable functional group onto the ethylene / C3-8 α-olefin copolymer. These introduction methods can be used alone or in appropriate combination. Among them, from the viewpoints of suppressing deterioration in the appearance of a film formed from the polyamide resin composition due to film gel and maintaining the transparency and good pinhole resistance of the film, it is preferable to produce copolymer (B) by method (ii) or (iii).
[0047] Examples of copolymerizable monomers having these functional groups and compounds having the functional group and a graftable functional group include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, crotonic acid, mesaconic acid, citraconic acid, glutaconic acid, cis-4-cyclohexene-1,2-dicarboxylic acid, endobicyclo-[2.2.1]-5-heptene-2,3-dicarboxylic acid and metal salts of these carboxylic acids, monomethyl maleate, monomethyl itaconate, methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, hydroxyethyl acrylate, and the like. Examples of suitable methacrylates include methyl methacrylate, 2-ethylhexyl methacrylate, hydroxyethyl methacrylate, aminoethyl methacrylate, dimethyl maleate, dimethyl itaconate, maleic anhydride, itaconic anhydride, citraconic anhydride, endobicyclo-[2.2.1]-5-heptene-2,3-dicarboxylic anhydride, maleimide, N-ethylmaleimide, N-butylmaleimide, N-phenylmaleimide, acrylamide, methacrylamide, glycidyl acrylate, glycidyl methacrylate, glycidyl ethacrylate, glycidyl itaconate, and glycidyl citraconate. These may be used alone or in combination of two or more. Among these, maleic anhydride, itaconic anhydride, or citraconic anhydride is preferred, maleic anhydride or itaconic anhydride is more preferred, and maleic anhydride is particularly preferred.
[0048] From the viewpoint of compatibility between polyamide and polyolefin and reduction of film gel, the functional group concentration in copolymer (B) is 1.0 to 60×10 -5 eq / g, and preferably 2.0 to 40×10 -5 eq / g, more preferably 3.0 to 30×10 -5 When the functional group of the copolymer (B) is a carboxyl group, an acid anhydride group, or a carboxylic acid ester group, the functional group concentration can be expressed as the equivalent of the carboxyl group per 1 g of the polymer, and is measured by neutralization titration with a 0.1 N KOH ethanol solution using a sample solution prepared using a solvent such as xylene and phenolphthalein as an indicator.
[0049] When copolymer (B) is a copolymer having groups derived from maleic anhydride by the above method (ii) or (iii), the maleic anhydride modification rate (content (mass %) of groups derived from maleic anhydride) is preferably 0.1% by mass to 3% by mass, more preferably 0.3% by mass to 2% by mass, and particularly preferably 0.5% by mass to 1.5% by mass. By setting the maleic anhydride modification rate within the above range, it is possible to improve the compatibility between polyamide and polyolefin and reduce film gel. The maleic anhydride modification rate can be measured by converting the equivalent of carboxyl groups obtained by the above neutralization titration into a maleic anhydride modification rate, or by measuring the wave number of 1780 cm assigned to carbonyl groups in FT-IR. -1 Examples of such a method include a method of measuring the peak intensity of the compound using a separately prepared calibration curve.
[0050] The copolymer (B) is an ethylene / α-olefin copolymer having 3 to 8 carbon atoms. From the viewpoints of suppressing deterioration in appearance of a film formed from the polyamide resin composition due to film gel and maintaining the transparency and good pinhole resistance of the film, it is preferable that the copolymer (B) does not contain a maleic anhydride monomer as a copolymerization component.
[0051] The α-olefin has 3 to 8 carbon atoms, preferably 4 to 6. Specific examples of α-olefins having 3 to 8 carbon atoms include 1-propene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, and 3-ethyl-1-hexene. These may be used alone or in combination of two or more. Among these, from the viewpoint of moldability, 1-propene, 1-butene, 1-hexene, and 1-octene are preferred, 1-propene, 1-butene, and 1-hexene are more preferred, and 1-hexene is particularly preferred.
[0052] From the viewpoint of compatibility between polyamide and polyolefin, in the copolymer (B), the proportion of the α-olefin monomer having 3 to 8 carbon atoms in the total of 100 mol % of the ethylene monomer and the α-olefin monomer having 3 to 8 carbon atoms constituting the copolymer is preferably 1 to 99 mol %, more preferably 5 to 95 mol %, and even more preferably 10 to 90 mol %.
[0053] The molecular structure of the copolymer (B) may be linear or branched having long or short side chains. The copolymer (B) may be selected from the group consisting of 1,4-pentadiene, 1,4-hexadiene, 1,5-hexadiene, 1,4-octadiene, 1,5-octadiene, 1,6-octadiene, 1,7-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, 7-methyl-1,6-octadiene, 4-ethylidene-8-methyl-1,7-nonadiene, 4,8-dimethyl-1,4,8-decatriene (DMDT), dicyclopentadiene, Polyenes such as non-conjugated dienes and non-conjugated trienes, such as cyclohexadiene, cyclooctadiene, 5-vinylnorbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, 6-chloromethyl-5-isopropenyl-2-norbornene, 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, and 2-propenyl-2,5-norbornadiene, may also be copolymerized. These may be used alone or in combination of two or more.
[0054] Among these, from the viewpoint of compatibility between the polyamide and the polyolefin, the copolymer (B) is preferably an ethylene / C3-8 α-olefin copolymer having a group derived from at least one selected from the group consisting of maleic anhydride and itaconic anhydride, more preferably an ethylene / propylene copolymer, ethylene / 1-butene copolymer, ethylene / 1-hexene copolymer, or ethylene / 1-octene copolymer having a group derived from maleic anhydride, even more preferably an ethylene / propylene copolymer, ethylene / 1-butene copolymer, or ethylene / 1-hexene copolymer having a group derived from maleic anhydride, even more preferably an ethylene / 1-butene copolymer or ethylene / 1-hexene copolymer having a group derived from maleic anhydride, still more preferably an ethylene / 1-butene copolymer or ethylene / 1-hexene copolymer having a group derived from maleic anhydride, and particularly preferably an ethylene / 1-hexene copolymer having a group derived from maleic anhydride.
[0055] From the viewpoint of moldability, the melting point of the copolymer (B) is preferably 70 to 120° C., more preferably 75 to 120° C., and even more preferably 80 to 115° C. The melting point is the melting peak temperature in a DSC curve obtained by heating the copolymer (B) to 280° C. in an air atmosphere, maintaining the temperature at this temperature for 5 minutes, then lowering the temperature to 0° C. at a rate of 20° C. / min, and then heating from 0° C. to 280° C. at a rate of 20° C. / min.
[0056] From the viewpoint of reducing film gel, the copolymer (B) preferably has a melt flow rate (MFR) measured in accordance with ASTM D1238 at 230°C under a load of 2.16 kg of 1 to 100 g / 10 min, more preferably 3 to 90 g / 10 min, and even more preferably 5 to 70 g / 10 min.
[0057] (Content of Copolymer (B)) The content of copolymer (B) is 1 to 5 mass% based on 100 mass% of the polyamide resin composition. By setting the content of copolymer (B) within this range, the aliphatic polyamide resin (A) and copolymer (B) exhibit good compatibility, improving the melt stability and film formability of the polyamide resin composition. Furthermore, deterioration of the appearance of polyamide films formed from the polyamide resin composition due to film gel can be suppressed, the transparency of the film can be maintained, and pinhole resistance in low-temperature environments can be improved. Furthermore, for laminate films containing at least a layer containing a polyamide resin composition and a layer containing a polyolefin, when waste film is recycled, the compatibility of the two layers is improved, improving the homogeneity of the recycled plastic raw material. The content of copolymer (B) is preferably 1.5 to 4.0 mass% based on 100 mass% of the polyamide resin composition, and more preferably 2.0 to 3.0 mass%. If the content of copolymer (B) in 100% by mass of the polyamide resin composition is less than 1% by mass, the pinhole resistance and friction coefficient of the molded film in a low-temperature environment will not improve, and material recyclability will deteriorate. If the content exceeds 5% by mass, the dispersibility of copolymer (B) in the polyamide resin composition will deteriorate, resulting in a decrease in transparency and an increase in film gel, and thus in a deterioration in the appearance and material recyclability of the film.
[0058] <Other Components (C)> The polyamide resin composition may contain another component (C) other than the components (A) and (B). Examples of the other components include polyamide resins other than the component (A), such as polyamide resins having an alicyclic or aromatic group in the main chain or side chain; thermoplastic resins other than the component (B); antioxidants, antiblocking agents, water repellents, lubricants, nucleating agents, plasticizers, foaming agents, stabilizers, UV absorbers, weather resistance agents, anti-fogging agents, colorants, etc. Among these, it is preferable that the polyamide resin composition contains a polyolefin (D) having no functional group, an antioxidant, a water repellent, and / or a lubricant.
[0059] The content of the other component (C) is 0 to 9 mass %, more preferably 0 to 5 mass %, and even more preferably 0 to 2 mass %, based on 100 mass % of the polyamide resin composition.
[0060] (Polyolefin (D) having no functional group (hereinafter also referred to as polyolefin (D))) The polyamide resin composition can contain polyolefin (D) having no functional group. Polyolefin (D) does not have a functional group such as those exemplified for copolymer (B). By containing polyolefin (D), pinhole resistance and material recyclability can be improved. Polyolefin (D) may be one type or a combination of two or more types.
[0061] Examples of the olefin in the polyolefin (D) include ethylene and α-olefins having 3 or more carbon atoms. Examples of the α-olefins having 3 or more carbon atoms include those exemplified for the copolymer (B). The polyolefin (D) may be a homopolymer or a copolymer of two or more olefins. The polyolefin (D) is preferably an ethylene homopolymer or a propylene homopolymer, and more preferably an ethylene homopolymer. Examples of ethylene homopolymers include high-density polyethylene (HDPE), medium-density polyethylene (MDPE), low-density polyethylene (LDPE), and linear low-density polyethylene (LLDPE). Among these, linear low-density polyethylene is preferred in terms of transparency, mechanical strength, and flexibility.
[0062] From the viewpoint of moldability, the polyolefin (D) preferably has a melt flow rate (MFR) measured in accordance with ASTM D1238 at 190°C under a load of 2.16 kg of 0.5 to 50 g / 10 min, more preferably 1 to 40 g / 10 min, and even more preferably 1 to 10 g / 10 min.
[0063] The content of polyolefin (D) is 0 to 9 mass%, preferably 2 to 8 mass%, and more preferably 2 to 5 mass%, based on 100 mass% of the polyamide resin composition. When the content of polyolefin (D) is within this range, the polyamide resin composition can have excellent mechanical strength, pinhole resistance, and material recyclability.
[0064] The polyamide resin composition can obtain antiblocking properties suitable for a film even without containing an antiblocking agent. From the viewpoints of economy and transparency, it is preferable that the polyamide resin composition is substantially free of an antiblocking agent, and from the viewpoint of transparency, it is more preferable that the polyamide resin composition is substantially free of silica. Here, "substantially free" means that the content of the antiblocking agent or silica in 100% by mass of the polyamide resin composition is less than 0.01% by mass, preferably less than 0.005% by mass, and more preferably less than 0.001% by mass.
[0065] To further improve the handleability of the formed film, the polyamide resin composition may contain an antiblocking agent. Examples of the antiblocking agent include minerals such as diatomaceous earth, calcium carbonate, feldspar, and quartz, synthetic silica, and crosslinked resin beads. The antiblocking agent may be one type or a combination of two or more types.
[0066] (Antioxidant) From the viewpoint of further reducing the amount of film gel generated and preventing yellowing during film formation and oxidative degradation during material recycling, the polyamide resin composition preferably contains an antioxidant. Examples of the antioxidant include organic antioxidants such as phenolic compounds, phosphorus compounds, and sulfur compounds, and inorganic antioxidants such as metal halide compounds. The antioxidant may be used alone or in combination of two or more.
[0067] The content of the antioxidant relative to 100% by mass of the polyamide resin composition is preferably 0.01 to 1% by mass, more preferably 0.02 to 0.8% by mass, and even more preferably 0.03 to 0.7% by mass.
[0068] (Compound (E)) The polyamide resin composition preferably contains compound (E), which is at least one selected from the group consisting of methylene bisstearamide, ethylene bisstearamide, butylene bisstearamide, and hexamethylene bisstearamide. Compound (E) may be one type or a combination of two or more types. A laminate film including a layer containing the polyamide resin composition can be produced by a molding method such as air-cooled inflation molding or water-cooled inflation molding. By containing compound (E) in the polyamide resin composition, it is possible to prevent a decrease in transparency of the laminate film due to water when using water-cooled inflation molding, and also to suppress hydrolysis of the composition due to water absorption during material recycling. Furthermore, compound (E) also functions as a lubricant.
[0069] The content of the compound (E) relative to 100% by mass of the polyamide resin composition is preferably 0.01 to 1% by mass, more preferably 0.02 to 0.8% by mass, and even more preferably 0.03 to 0.7% by mass.
[0070] (Compound (F)) The polyamide resin composition preferably contains compound (F), which is at least one selected from the group consisting of terminally modified polyalkylene glycols, phosphate esters or phosphites, higher fatty acid monoesters, higher fatty acids, metal salts of higher fatty acids, higher fatty acid monoamides, N-substituted higher fatty acid monoamides, magnesium silicate, and substituted benzylidene sorbitols. In this specification, "higher fatty acid" refers to a fatty acid having 6 or more carbon atoms. Compound (F) may be one type or a combination of two or more types. Compound (F) functions as a lubricant, and by including compound (F) in the polyamide resin composition, it is possible to improve the slipperiness between pellets before molding, between a processing machine and the pellets, or between molded films. Among these, from the viewpoint of improving the slipperiness between a processing machine and the pellets, metal salts of higher fatty acids are preferred, metal salts of stearic acid are more preferred, and magnesium stearate or calcium stearate are even more preferred. Furthermore, the use of metal salts of stearic acid is preferred because it has the effect of suppressing gel formation during material recycling.
[0071] The content of the compound (F) relative to 100% by mass of the polyamide resin composition is preferably 0.01 to 1% by mass, more preferably 0.02 to 0.8% by mass, and even more preferably 0.03 to 0.7% by mass.
[0072] [Physical Properties of Polyamide Resin Composition] The polyamide resin composition has a number-average molecular weight (Mn) of 50,000 to 60,000 as measured by GPC. By setting the Mn of the polyamide resin composition within this range, the occurrence of film gels in polyamide films molded from the polyamide resin composition can be suppressed. The number-average molecular weight (Mn) is more preferably 53,000 to 60,000, and even more preferably 55,000 to 60,000. Furthermore, the ratio of the weight-average molecular weight (Mw) to the number-average molecular weight (Mn) of the polyamide resin composition as measured by GPC (Mw / Mn) is preferably 1.5 to 3.0, more preferably 1.5 to 2.8, and even more preferably 1.6 to 2.5. The Mn and Mw values are measured by gel permeation chromatography (GPC).
[0073] The polyamide resin composition is heated to 280°C in an air atmosphere, held at this temperature for 5 minutes, then cooled to 0°C at a rate of 20°C / min, and then heated from 0°C to 280°C at a rate of 20°C / min. The DSC curve shows a melting peak in the range of 150 to 205°C. This melting peak is derived from the aliphatic polyamide resin (A). Having such a melting peak can improve material recyclability. Specifically, for a laminate film containing at least a layer containing a polyamide resin composition and a layer containing a polyolefin, when waste from the film is recycled, it is possible to suppress an increase in the melt-kneading temperature when the waste is melt-kneaded and processed into pellets, etc., thereby preventing discoloration and thermal degradation due to excessive heating of the polyolefin contained in the waste and improving the performance of the resulting recycled product. The melting peak temperature is more preferably 150 to 200°C, and even more preferably 160 to 198°C.
[0074] If the melting peak in the DSC curve is less than 150°C, the mechanical strength of the molded article will be deteriorated. If the melting peak in the DSC curve is more than 205°C, the material recyclability will be deteriorated. Specifically, for a laminate film including at least a layer containing a polyamide resin composition and a layer containing a polyolefin, when waste of the film is recycled, if the melting peak is more than 205°C, excessive heating will be required when the waste is melt-kneaded and processed into pellets or the like, resulting in discoloration, thermal degradation, etc. of the polyolefin contained in the waste.
[0075] The polyamide resin composition preferably further exhibits a melting peak temperature in the range of 70 to 120°C in a DSC curve obtained by heating the composition in an air atmosphere to 280°C, holding the composition at that temperature for 5 minutes, subsequently lowering the temperature to 0°C at a rate of 20°C / min, and then heating the composition from 0°C to 280°C at a rate of 20°C / min. This melting peak is derived from the copolymer (B) and / or polyolefin (D). Having such a melting peak can improve moldability and the strength of molded articles. The melting peak temperature is preferably in the range of 74 to 120°C, more preferably in the range of 78 to 113°C.
[0076] [Method for Producing Polyamide Resin Composition] The method for producing the polyamide resin composition is not particularly limited. For example, the following Production Methods 1 and 2 can be applied as the method for producing the polyamide resin composition.
[0077] (Production Method 1) A polyamide resin composition is obtained by melt-kneading an aliphatic polyamide resin (A) and a copolymer (B) in a kneader. The polyamide resin composition may contain another component (C). Examples of kneaders include single-screw and twin-screw extruders, Banbury mixers, kneaders, and mixing rolls. For example, any of the following methods may be used: a twin-screw extruder is used to blend all raw materials and then melt-knead them; or a side feeder is used to blend some raw materials and then mix the remaining raw materials during melt-kneading. When the polyamide resin composition is melted in a film-forming machine or the like and processed into a film, it is preferably processed into pellets in advance from the viewpoints of film production stability and dispersibility of each component in the polyamide resin composition.
[0078] (Production Method 2) The first aliphatic polyamide resin (a1) and the copolymer (B) are melt-kneaded in a kneader to obtain a melt-kneaded product (G). A second aliphatic polyamide resin (a2) is prepared separately. The melt-kneaded product (G) and the first and second aliphatic polyamide resins may each be blended with other components (C). The melt-kneaded product (G) and the second aliphatic polyamide resin (a2) may each be formed into pellets, and then these pellets and, if necessary, other components (C) may be uniformly dry-blended to a specific ratio using, for example, a tumbler, a mixer, or the like to obtain a pellet mixture. A polyamide resin composition can also be obtained by melt-kneading these pellet mixtures in a kneader. The kneaders exemplified in Production Method 1 can be used as the kneader. It is particularly preferred to produce a polyamide resin composition by melt-kneading such a pellet mixture in a single-screw extruder. The copolymer (B) is melt-kneaded with the first aliphatic polyamide resin (a1) to produce a melt-kneaded product (G), which is then pelletized and dry-blended with pellets of the second aliphatic polyamide resin (a2) to produce a pellet mixture, thereby improving the dispersibility of the copolymer (B) in the polyamide resin composition obtained by melt-kneading. The improved dispersibility of the copolymer (B) is thought to contribute to improving the formability of the film, improving the pinhole resistance of the film in a low-temperature environment, and reducing film gels.
[0079] When the other component (C) contains a polyolefin (D) having no functional group, the first pellets containing the melt-kneaded product (G) may contain the polyolefin D. Alternatively, a third pellet containing the polyolefin (D) may be prepared in addition to the first pellets containing the melt-kneaded product (G) and the second pellets containing the second aliphatic polyamide resin (a2), and these pellets may be uniformly dry-blended to a specific ratio to obtain a pellet mixture. The pellet mixture may also be melt-kneaded in a kneader to obtain a polyamide resin composition. The dry-blending and melt-kneading methods are as described above.
[0080] [Pellet Mixture] When producing a polyamide resin composition by the above-mentioned Production Method 2, it is preferable to use a pellet mixture containing first pellets containing a first aliphatic polyamide resin (a1) and a functional group-containing ethylene / α-olefin copolymer (B) having 3 to 8 carbon atoms (hereinafter also referred to as copolymer (B)); and second pellets containing a second aliphatic polyamide resin (a2). Note that the second pellets are not the first pellets. That is, the polyamide resin compositions constituting the first pellets and the second pellets are different from each other. The second pellets may contain less than 1.0 mass% of copolymer (B) per 100 mass% of the second pellets, but preferably do not contain copolymer (B). The first pellets and the second pellets may each be one type or a combination of two or more types.
[0081] The first pellets and the second pellets may each contain other components (C) such as a polyolefin (D) having no functional groups, an antioxidant, a compound (E), or a compound (F). It is preferable that the second pellets do not contain the polyolefin (D) having no functional groups. The pellet mixture may also contain other components (C) such as a polyolefin (D) having no functional groups, an antioxidant, a compound (E), or a compound (F) in addition to the first pellets and the second pellets. In this case, the polyolefin (D) having no functional groups is preferably contained in the pellet mixture as the third pellets.
[0082] In the first aliphatic polyamide resin (a1) and the second aliphatic polyamide resin (a2), the ratio of the number of methylene groups to the number of amide groups is 3 or more and 11 or less. The aliphatic polyamide resin (a1) and the aliphatic polyamide resin (a2) can be the polyamide resins exemplified for the aliphatic polyamide resin (A). The aliphatic polyamide resin (a1) and the aliphatic polyamide resin (a2) may be the same or different, but are preferably different. The aliphatic polyamide resin (a1) and the aliphatic polyamide resin (a2) may each be one type or a combination of two or more types.
[0083] (First pellets) From the viewpoint of melt stability during melt-kneading in the production of the first pellets, the content of the first aliphatic polyamide resin (a1) is preferably 60 to 90% by mass relative to 100% by mass of the first pellets. From the viewpoint of reducing film gels, the content of the first aliphatic polyamide resin (a1) is more preferably 65% by mass or more, and even more preferably 68% by mass or more, relative to 100% by mass of the first pellets. Furthermore, from the viewpoint of improving mechanical properties, the content of the first aliphatic polyamide resin (a1) is more preferably 88% by mass or less, and even more preferably 85% by mass or less, relative to 100% by mass of the first pellets.
[0084] From the viewpoints of compatibility with the copolymer (B) and the transparency of the resulting film, the aliphatic polyamide resin (a1) is preferably an aliphatic homopolyamide, more preferably polyamide 6 or polyamide 66, and particularly preferably polyamide 6.
[0085] The copolymer (B), including preferred embodiments thereof, is as described above. From the viewpoint of moldability, the melting point of the copolymer (B) is preferably 70 to 120°C, more preferably 75 to 120°C, and even more preferably 80 to 115°C. The melting point is the melting peak temperature in a DSC curve obtained by heating the copolymer (B) to 280°C in an air atmosphere, maintaining the temperature at this temperature for 5 minutes, then lowering the temperature to 0°C at a rate of 20°C / min, and then heating from 0°C to 280°C at a rate of 20°C / min.
[0086] From the viewpoints of pinhole resistance and material recyclability of film waste, the content of copolymer (B) is preferably 10 to 40% by mass relative to 100% by mass of the first pellets. From the viewpoints of pinhole resistance and material recyclability of film waste, the content of copolymer (B) is more preferably 12% by mass or more, and even more preferably 15% by mass or more. Furthermore, from the viewpoints of film transparency and film gel, the content of copolymer (B) is more preferably 35% by mass or less, and even more preferably 32% by mass or less, relative to 100% by mass of the first pellets.
[0087] From the viewpoint of molding processability, the content of the other component (C) is preferably 0 to 9% by mass based on 100% by mass of the first pellets. The content of the other component (C) is more preferably 3% by mass or less, and even more preferably 1% by mass or less. Furthermore, the content of the other component (C) is more preferably 0.1% by mass or more, and even more preferably 0.2% by mass or more based on 100% by mass of the first pellets. The first pellets preferably contain an antioxidant, a compound (E), and / or a compound (F) as the other component (C).
[0088] From the viewpoint of film formability, the MFR of the first pellets, measured in accordance with ASTM D1238 at 230°C under a load of 2.16 kg, is preferably 1 to 40 g / 10 min. The MFR of the first pellets is more preferably 2 g / 10 min or more, even more preferably 3 g / 10 min or more, and particularly preferably 4 g / 10 min or more. The MFR of the first pellets is more preferably 35 g / 10 min or less, and even more preferably 30 g / 10 min or less.
[0089] From the viewpoint of pinhole resistance of the molded polyamide film in a low-temperature environment, the content of the first pellets is preferably 2% by mass or more, more preferably 4% by mass or more, and even more preferably 6% by mass or more, based on 100% by mass of the pellet mixture. Also, from the viewpoint of dispersibility of each component in the polyamide resin composition, the content of the first pellets is preferably 25% by mass or less, more preferably 20% by mass or less, even more preferably 15% by mass or less, even more preferably 12% by mass or less, and particularly preferably 11.5% by mass or less, based on 100% by mass of the pellet mixture.
[0090] (Second pellets) The second pellets contain a second aliphatic polyamide resin (a2). The content of the second aliphatic polyamide resin (a2) is preferably 95 to 100 mass%, more preferably 97 to 100 mass%, and even more preferably 99 to 100 mass%, based on 100 mass% of the second pellets.
[0091] The second pellets may contain less than 1.0% by mass of the copolymer (B) based on 100% by mass of the second pellets. In a preferred embodiment, the second pellets do not contain the copolymer (B).
[0092] The second aliphatic polyamide resin (a2) preferably contains 0 to 20 mass% of an aliphatic homopolyamide and 80 to 100 mass% of an aliphatic copolyamide, based on 100 mass% of the aliphatic polyamide resin (a2). More preferably, the aliphatic polyamide resin (a2) contains only an aliphatic copolyamide.
[0093] In the aliphatic polyamide resin (a2), the aliphatic copolyamide is preferably selected from the group consisting of polyamide 6 / 66, polyamide 6 / 69, polyamide 6 / 11, polyamide 6 / 12, polyamide 6 / 66 / 11, and polyamide 6 / 66 / 12, and particularly preferably polyamide 6 / 66.
[0094] From the viewpoint of molding processability, the content of the other component (C) is preferably 5% by mass or less, more preferably 0 to 3% by mass, and even more preferably 0 to 1% by mass, based on 100% by mass of the second pellets. The second pellets preferably contain an antioxidant, a compound (E) and / or a compound (F) as the other component (C).
[0095] The second aliphatic polyamide resin (a2) preferably has a relative viscosity of 2.5 to 5.0, as measured at 25°C by dissolving 1 g of polyamide resin in 100 ml of 96% sulfuric acid in accordance with JIS K 6920. By setting the relative viscosity of the second aliphatic polyamide resin (a2) within the above range, film formability can be improved. The relative viscosity of the second aliphatic polyamide resin (a2) is more preferably 2.8 or higher, and even more preferably 2.9 or higher. The relative viscosity of the second aliphatic polyamide resin (a2) is more preferably 4.5 or lower, and even more preferably 4.1 or lower.
[0096] When the second aliphatic polyamide resin (a2) is a combination of two or more types, it is preferable to measure the relative viscosity by the above-mentioned method. However, when the relative viscosity of each polyamide resin and its mixing ratio are known, the relative viscosity of the second aliphatic polyamide resin (a2) may be determined by adding up the values obtained by multiplying each relative viscosity by the mixing ratio.
[0097] From the viewpoints of molding processability and material recyclability of film waste, the melting point of the second aliphatic polyamide resin (a2) is preferably 150 to 205° C., more preferably 150 to 200° C. The melting point is the melting peak temperature in a DSC curve obtained by heating the second aliphatic polyamide resin (a2) to 280° C. in an air atmosphere, maintaining the temperature at this temperature for 5 minutes, then lowering the temperature to 0° C. at a rate of 20° C. / min, and then heating from 0° C. to 280° C. at a rate of 20° C. / min.
[0098] From the viewpoint of film forming processability, the MFR of the second aliphatic polyamide resin (a2) measured in accordance with ASTM D1238 at 230°C under a load of 2.16 kg is preferably 1 to 20 g / 10 min, more preferably 1 to 18 g / 10 min, and even more preferably 2 to 15 g / 10 min.
[0099] From the viewpoint of film transparency, the content of the second pellets is preferably 66% by mass or more, more preferably 72% by mass or more, even more preferably 80% by mass or more, and particularly preferably 83.5% by mass or more, based on 100% by mass of the pellet mixture. From the viewpoint of pinhole resistance, the content of the second pellets is preferably 98% by mass or less, more preferably 96% by mass or less, and even more preferably 94% by mass or less, based on 100% by mass of the pellet mixture.
[0100] (Aliphatic homopolyamide and aliphatic copolyamide content) In the first pellets and the second pellets, the content of the aliphatic homopolyamide is 1 to 50 mass%, and the content of the aliphatic copolyamide is 50 to 99 mass%, relative to 100 mass% of the total of the first aliphatic polyamide resin (a1) and the second aliphatic polyamide resin (a2). By setting the content of the aliphatic homopolyamide and the aliphatic copolyamide within the above ranges, the transparency, flexibility, and stretchability of the resulting film can be improved. The content of the aliphatic homopolyamide relative to 100 mass% of the total of the aliphatic polyamide resin (a1) and the aliphatic polyamide resin (a2) is preferably 3 to 30 mass%, more preferably 4 to 20 mass%, and particularly preferably 5 to 15 mass%. The content of the aliphatic copolyamide relative to the total of the aliphatic polyamide resin (a1) and the aliphatic polyamide resin (a2) (100% by mass) is preferably 70 to 97% by mass, more preferably 80 to 96% by mass, and particularly preferably 85 to 95% by mass.
[0101] (Third pellets) When the polyamide resin composition contains a polyolefin (D) having no functional group as the other component (C), the pellet mixture may contain, in addition to the first pellets and the second pellets, third pellets containing the polyolefin (D). In this case, it is preferable that the first pellets and the second pellets do not contain the polyolefin (D). By including the third pellets in the pellet mixture, the pinhole resistance of the film is improved. The third pellets may be one type or a combination of two or more types.
[0102] The content of the polyolefin (D) is preferably 95 to 100 mass%, more preferably 97 to 100 mass%, and even more preferably 99 to 100 mass%, based on 100 mass% of the third pellets. The third pellets may contain an antioxidant, a compound (E) and / or a compound (F) as other component (C).
[0103] From the viewpoints of mechanical strength, pinhole resistance, and material recyclability, the content of the third pellets is preferably 0 to 9% by mass, more preferably 2 to 8% by mass, and even more preferably 2 to 5% by mass, relative to 100% by mass of the pellet mixture. The content of the third pellets can be 0% by mass or more, and more preferably 2% by mass or more, relative to 100% by mass of the pellet mixture. Furthermore, the content of the third pellets is preferably 9% by mass or less, more preferably 8% by mass or less, and even more preferably 5% by mass or less, relative to 100% by mass of the pellet mixture.
[0104] (Pellet Mixture) The total content of the first aliphatic polyamide resin (a1) and the second aliphatic polyamide resin (a2) is preferably 88 to 99% by mass, more preferably 89 to 98% by mass, based on 100% by mass of the kneaded product obtained after melt-kneading the pellet mixture. By setting the total content of the first aliphatic polyamide resin (a1) and the second aliphatic polyamide resin (a2) within the above range, the aliphatic polyamide resin (A) and the copolymer (B) exhibit good compatibility, improving the melt stability and film formability of the polyamide resin composition. Furthermore, deterioration of the appearance of a polyamide film formed from the polyamide resin composition due to film gel can be suppressed, and the transparency and good pinhole resistance of the film can be maintained. Furthermore, the material recyclability of the film waste is also improved.
[0105] The content of copolymer (B) is preferably 1 to 5% by mass, more preferably 1.5 to 4.0% by mass, and even more preferably 2.0 to 3.0% by mass, based on 100% by mass of the kneaded product obtained after melt-kneading the pellet mixture. By setting the content of copolymer (B) within the above range, the aliphatic polyamide resin (A) and copolymer (B) exhibit good compatibility, improving the melt stability and film formability of the polyamide resin composition. Furthermore, deterioration of the appearance of polyamide films formed from the polyamide resin composition due to film gel can be suppressed, the transparency of the film can be maintained, and pinhole resistance in low-temperature environments can be improved. Furthermore, for laminate films containing at least a layer containing a polyamide resin composition and a layer containing a polyolefin, when waste film is recycled, the compatibility of the two layers is improved, improving the homogeneity of the recycled plastic raw material.
[0106] From the viewpoint of molding processability, the content of the other component (C) is preferably 0 to 9 mass%, more preferably 0 to 5 mass%, and even more preferably 0 to 2 mass%, based on 100 mass% of the kneaded product obtained after melt-kneading the pellet mixture.
[0107] When the pellet mixture contains the third pellets, from the viewpoints of mechanical strength, pinhole resistance, and material recyclability, the content of the polyolefin (D) is preferably 2 to 8 mass%, more preferably 2 to 5 mass%, based on 100 mass% of the kneaded product obtained after melt-kneading the pellet mixture.
[0108] From the viewpoint of reducing film gels, the number average molecular weight Mn of the kneaded product obtained by melt-kneading the pellet mixture, as measured by GPC, is preferably 50,000 to 60,000, more preferably 53,000 to 60,000, and even more preferably 55,000 to 60,000. Furthermore, the ratio of the weight average molecular weight Mw to the number average molecular weight Mn (Mw / Mn), as measured by GPC, of the kneaded product obtained by melt-kneading the pellet mixture, is preferably 1.5 to 3.0, more preferably 1.5 to 2.8, and even more preferably 1.6 to 2.5. The Mn and Mw values are measured by gel permeation chromatography (GPC).
[0109] The pellet mixture can be melt-kneaded to obtain a polyamide resin composition. The preferred range of the melting peak temperature of the polyamide resin composition thus obtained is as described above.
[0110] Another aspect of the invention is the first pellet for use in admixture with the second pellet in the production of a pellet mixture. Yet another aspect of the invention is the second pellet for use in admixture with the first pellet in the production of a pellet mixture.
[0111] (Production of Pellets) The pellets can be obtained, for example, by extruding the polyamide resin composition in the form of strands from an extruder or the like, and cutting the strands with a cutter having a rotary blade.
[0112] The pellets may have a shape such as a sphere, a strip, a spheroid, a shape slightly deformed from an exact spheroid, a cylindrical shape with a circular or elliptical cross section, etc. Among these, the pellets are preferably spherical, spheroidal, or cylindrical with a circular or elliptical cross section.
[0113] When the pellet has an elliptical cross section, its major axis is preferably 1 to 5 mm, more preferably 2 to 4 mm, and even more preferably 2.0 to 3.5 mm. When the pellet has an elliptical cross section, its minor axis is preferably 1 to 3 mm, and more preferably 2 to 3 mm. The ratio of the major axis to the minor axis (major axis / minor axis) is not particularly limited, but is preferably 1 to 4.
[0114] The major and minor diameters of the pellets can be controlled, for example, by adjusting the diameter of the nozzle of an extruder or the like to change the diameter of the strands.
[0115] The length of the pellet is not particularly limited, but is preferably 2 to 4 mm, and more preferably 2.5 to 4.0 mm.
[0116] [Polyamide Film] The polyamide film contains a polyamide resin composition. The polyamide film may be an unstretched polyamide film or a stretched polyamide film obtained by stretching the unstretched polyamide film. From the viewpoint of mechanical strength, a stretched polyamide film is preferable.
[0117] The method for producing the polyamide film is not particularly limited, and for example, known production methods can be applied. For example, a polyamide film can be produced by melt-kneading the polyamide resin composition obtained by Production Method 1 using an extruder, extruding it into a film using a die such as a T-die or a coat hanger die, casting it on a casting roll surface, and then cooling it. Alternatively, according to Production Method 2, the melt-kneaded product (G) or the first pellets, the aliphatic polyamide resin (a2) or the second pellets, and any other components can be melt-kneaded using an extruder to produce a polyamide film in the same manner. Furthermore, the pellet mixture can also be melt-kneaded using an extruder or the like to produce a polyamide film in the same manner.
[0118] The produced polyamide film may be stretched to form a stretched film. In this case, the produced polyamide film may be uniaxially stretched to form a uniaxially stretched film, or biaxially stretched (simultaneous biaxial stretching or sequential biaxial stretching) to form a biaxially stretched film. The stretching method is not particularly limited, and examples include uniaxial stretching using a heated roll, simultaneous biaxial stretching using a tubular method, and sequential biaxial stretching using a heated roll and a tenter. The temperature of the heated roll is not particularly limited and can be set in the range of 35°C to 130°C, and can be appropriately selected depending on the material of the polyamide film and the desired stretch ratio. The stretch ratio includes the stretch ratio in the extrusion direction (MD) of the film and the direction perpendicular to the extrusion direction (TD) of the film. The stretch ratio in the extrusion direction of the film is not particularly limited, but is preferably 2 times or more, more preferably 2 to 6 times, and particularly preferably 2.5 to 5 times. The stretching ratio in the direction perpendicular to the extrusion direction of the film is not particularly limited, but is preferably 2 times or more, more preferably 2 to 6 times, and particularly preferably 2.5 to 5 times. The stretching ratio can be adjusted depending on the purpose.
[0119] The thickness of the film is not particularly limited and may be appropriately selected depending on the purpose, etc. In the case of a single-layer polyamide film, the thickness of the film can be, for example, 10 μm to 300 μm in the case of an unstretched film, and 5 μm to 100 μm in the case of a stretched film.
[0120] Polyamide films exhibit excellent pinhole resistance. Specifically, pinhole resistance can be evaluated by performing a 1,000-cycle flex test at 5°C on an unstretched polyamide film using a Gelbo Flex Tester (manufactured by Tester Sangyo Co., Ltd.) in accordance with MIL-B-131C, then placing the film on a recording paper, applying India ink, and counting the number of black dots recorded on the recording paper. If the number of counted black dots is 110 or less per 0.03 m, the pinhole resistance can be evaluated. 2 and more preferably 80 or less / 0.03 m 2 and more preferably 70 or less per 0.03 m 2 is.
[0121] The haze ratio of the polyamide film is preferably 25% or less, more preferably 15% or less, and even more preferably 10% or less, as measured in accordance with ASTM D-1003.
[0122] The polyamide film preferably has a gloss value of 50% or more, more preferably 80% or more, and even more preferably 100% or more, where the gloss value of the polyamide film is measured in accordance with ASTM D-523.
[0123] [Laminate Film] The laminate film includes at least one layer containing a polyamide resin composition (also referred to as a polyamide film layer). Examples of methods for producing the laminate film include a method including a step of laminating an additional layer on one or both sides of the polyamide film. The lamination method is not particularly limited, and examples include the coextrusion method, extrusion lamination method, and dry lamination method described in JP 2011-225870 A, with the coextrusion method being preferred from an economical standpoint. The produced laminate film may be stretched to form a stretched laminate film. In this case, the produced laminate film may be uniaxially stretched to form a uniaxially stretched film laminate, or biaxially stretched (simultaneous biaxial stretching or sequential biaxial stretching) to form a biaxially stretched film laminate. The stretching method and stretch ratio are as described in the section on polyamide film.
[0124] (Blown film molding) The laminated film can be produced by a molding method such as air-cooled blown film molding or water-cooled blown film molding. Of these, the air-cooled blown film molding requires simple equipment and allows the film width to be easily changed simply by adjusting the blow ratio, resulting in good workability and high productivity in film production.
[0125] The conditions for forming a film by air-cooled inflation extrusion are not particularly limited, but the forming temperature is preferably equal to or higher than the melting point of the raw resin used but less than 300°C. The forming temperature can be, for example, 230°C to 260°C. The blow-up ratio refers to the ratio of the maximum bubble diameter to the die diameter, and is preferably 1.1 to 3.0, more preferably 1.2 to 2.5. The take-up speed is determined by the thickness, width, and extrusion rate of the film, and can be adjusted within a range that maintains film formation stability. In general, the take-up speed is preferably 1 to 150 m / min, more preferably 5 to 100 m / min.
[0126] (Additional Layer) The additional layer is not particularly limited as long as the laminated film exhibits the effects of a polyamide film, and examples thereof include a polyolefin layer and an adhesive layer. Here, the adhesive layer is appropriately selected for the purpose of improving the adhesion and formability between the polyamide film layer and the polyolefin layer according to the present invention. Note that the polyamide film layer according to the present invention is not a polyolefin layer or an adhesive layer.
[0127] The polyolefin layer and the adhesive layer may contain additives, such as those exemplified as the other component (C).
[0128] Examples of polyolefins constituting the polyolefin layer include non-polar polyolefins such as low-density polyethylene, linear low-density polyethylene, high-density polyethylene, ethylene / α-olefin copolymers having 3 or more carbon atoms, propylene homopolymers, and propylene / α-olefin copolymers having 4 or more carbon atoms, as well as ethylene / acrylic acid copolymers, ethylene / vinyl acetate copolymers, ethylene / acrylic acid ester copolymers, and ethylene / methacrylic acid copolymers. Among these, from the viewpoint of food packaging applications, non-polar polyolefins and ethylene / vinyl acetate copolymers are preferred, and linear low-density polyethylene is more preferred. When the polyolefin layer is a non-polar polyolefin layer, the water vapor barrier properties of the laminate film tend to be further improved. When the polyolefin layer is an ethylene / vinyl acetate copolymer layer, the oxygen gas permeability of the laminate film tends to be further reduced. A laminate film comprising at least a polyamide film layer and a polyolefin layer is not only suitable for food packaging but also exhibits excellent material recyclability for waste film.
[0129] The adhesive layer is composed of an adhesive resin or adhesive. Examples of adhesive resins include acid-modified polyolefin resins such as acid-modified polyethylene grafted with at least one monomer selected from unsaturated carboxylic acids and their derivatives, such as maleic acid-modified polyethylene, ionomers, ethylene / acrylic acid copolymers, ethylene / methacrylic acid copolymers, etc. Examples of adhesives include solvent-based adhesives and solventless adhesives, and include those that bond with one liquid as well as those that bond by mixing two liquids. Examples of adhesives include epoxy-based adhesives and urethane-based adhesives, with urethane-based adhesives being preferred. Examples of urethane-based adhesives include aromatic ether-based, aliphatic ester-based, and aromatic ester-based adhesives.
[0130] (Layer Structure) Specific layer structures of the laminate film include two layers consisting of a polyamide film layer and a polyolefin layer; three layers consisting of a polyamide film layer / adhesive layer / polyolefin layer; at least three layers consisting of a polyamide film layer and a polyolefin layer, and one or more additional layers selected from the group consisting of a polyamide film layer, an adhesive layer, and a polyolefin layer; and at least four layers consisting of a polyamide film layer, a polyolefin layer, and an adhesive layer, and one or more additional layers selected from the group consisting of a polyamide film layer, an adhesive layer, and a polyolefin layer. Among these, from the viewpoint of food packaging applications, a laminate film containing at least three layers, in which a layer containing a polyamide resin composition, an adhesive layer, and a polyolefin layer are laminated in this order, or a laminate film containing at least five layers, in which an adhesive layer and a polyolefin layer are laminated in this order on both sides of a layer containing a polyamide resin composition, respectively. Furthermore, when the laminate film is an unstretched laminate film and a deep-draw packaging film, it is preferable that the polyolefin layer be an inner layer. Here, in the laminate film, the layer in contact with the outside air is the outer layer, and the layer in contact with the packaged food is the inner layer. The layer containing the polyamide resin composition may be a biaxially stretched layer.
[0131] (Thickness) The thickness of the laminate film is not particularly limited and can be selected depending on the application. The thickness of each polyamide film layer in the laminate film can be 1 to 300 μm, preferably 2 to 100 μm, and more preferably 5 to 80 μm. The thickness of each polyolefin layer can be selected appropriately depending on the purpose and is preferably in the range of, for example, 8 to 120 μm. The thickness of each adhesive layer can be selected depending on the purpose and is preferably in the range of, for example, 1 to 100 μm. The total thickness of the laminate film is not particularly limited and is preferably 5 to 500 μm, more preferably 20 to 300 μm, and particularly preferably 50 to 200 μm.
[0132] [Uses] The polyamide resin composition and the pellet mixture can be used as raw materials for various molded products. Molded products containing the polyamide resin composition can be used in a wide range of applications, such as packaging films for food packaging, automobile parts, computers and related equipment, optical equipment parts, electrical and electronic equipment, information and communication equipment, precision equipment, civil engineering and construction supplies, medical supplies, and household goods, and are suitable for packaging films, and are particularly useful for food packaging films.
[0133] The polyamide film and laminate film are free from the deterioration of appearance caused by film gel and have excellent pinhole resistance in low-temperature environments, making them suitable for use in packaging goods, particularly food packaging.
[0134] Unstretched polyamide films and unstretched laminated films have excellent deep drawability and are therefore suitable for use as food packaging films, particularly as films for deep draw packaging of foods. When an unstretched polyamide film is used as a deep draw packaging film, the food is placed in a deep draw packaging base material obtained by deep drawing the film, and packaged using a lid material. Examples of foods that can be placed in deep draw packaging base materials include sliced foods such as ham and cheese. The lid material is not particularly limited and can be selected appropriately depending on the purpose.
[0135] Stretched polyamide films and stretched laminated films have excellent mechanical strength and oxygen barrier properties, and are therefore useful as food packaging films for filling and packaging semi-liquid foods such as sausages (paste products) and solid foods such as processed meats and hams.
[0136] In particular, laminate films comprising at least a layer containing a polyamide resin composition and a polyolefin layer, and laminate films in which a layer containing a polyamide resin composition, an adhesive layer and a polyolefin layer are laminated in this order, are not only suitable for use in food packaging, but are also useful because they have excellent material recyclability for the film waste.
[0137] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited to these examples and can be practiced with appropriate modifications within the scope of the present invention.
[0138] [Measurement of physical properties of each raw material, first to third pellets, and polyamide resin composition] The following physical properties were evaluated for each raw material, first to third pellets, and polyamide resin composition. 1. Relative viscosity For aliphatic polyamide resin (A), 1 g of polyamide resin was dissolved in 100 ml of 96% sulfuric acid in accordance with JIS K 6920, and the relative viscosity at 25°C was measured.
[0139] 2. DSC Measurement (1) Each Raw Material Measurement was performed on each raw material using a differential scanning calorimeter (DSC). The sample was heated to 280°C at a rate of 20°C / min in an air atmosphere, held at this temperature for 5 minutes, then cooled to 0°C at a rate of 20°C / min, and then heated from 0°C to 280°C at a rate of 20°C / min. The top temperature of the endothermic peak during the second heating was recorded as the melting peak temperature (melting point). (2) Polyamide Resin Composition Measurement was performed on the polyamide resin composition using a differential scanning calorimeter (DSC). The sample was heated to 280°C at a rate of 20°C / min in an air atmosphere, held at this temperature for 5 minutes, and then cooled to 0°C at a rate of 20°C / min. The top temperature of the exothermic peak when the temperature was lowered to 0°C was recorded as the crystallization temperature. The sample was then heated from 0°C to 280°C at a rate of 20°C / min. The top temperature of the endothermic peak during the second temperature increase was taken as the melting peak temperature (melting point).
[0140] 3. MFR (230°C and 2.16 kg load) The MFR of the aliphatic polyamide resin (A) and the acid-modified ethylene / α-olefin copolymer (B) was measured at 230°C and a load of 2.16 kg in accordance with ASTM D 1238. The MFR of the polyolefin (D) having no functional group was also measured at 190°C and a load of 2.16 kg in accordance with ASTM D 1238.
[0141] 4. Terminal Amino Group Concentration For aliphatic polyamide resin (A), a predetermined amount of polyamide resin was placed in an Erlenmeyer flask equipped with a stopcock, and 40 mL of a previously prepared solvent: phenol / methanol (volume ratio 7 / 3) was added. After that, the resin was stirred with a magnetic stirrer to dissolve, and titration was carried out with 1 / 50 N hydrochloric acid using thymol blue as an indicator to determine the terminal amino group concentration (eq / g).
[0142] 5. Molecular Weight by GPC Measurement GPC measurement was performed using HLC-8320GPO manufactured by Tosoh Corporation under the following conditions, and the number average molecular weight Mn and weight average molecular weight Mw of the polyamide resin composition were calculated in terms of PMMA. Column: TSKgel Super AW3000 + TSKgel Super AW5000 Eluent: 10 mM CF 3 COOHNa / TFE Detector: RI Temperature: 40°C Flow rate: Sample 0.3 ml / min, Reference 0.15 ml / min Sample concentration: Approximately 0.1 wt / vol% Injection volume: 20 μl
[0143] [Materials Used] The materials used in the Examples and Comparative Examples are as follows: (1) Aliphatic Polyamide Resin (A) Polyamide Resin (A-1): Polyamide 6, manufactured by UBE Corporation (relative viscosity: 2.2; melting point: 220°C; MFR measured in accordance with ASTM D1238 at 230°C and a load of 2.16 kg: 60.0 g / 10 min; terminal amino group concentration: 3.3 x 10) -5 Polyamide resin (A-2): a copolymer of polyamide 6 and polyamide 66, manufactured by UBE Corporation (copolymerization ratio (by mass): polyamide 6:polyamide 66=80% by mass:20% by mass; relative viscosity: 4.0; melting point: 192°C; terminal amino group concentration: 3.5×10 -5 eq / g); MFR measured in accordance with ASTM D1238 at 230°C and a load of 2.16 kg: 3.9 g / 10 min. Polyamide resin (A-3): Polyamide 6, manufactured by UBE Co., Ltd. (relative viscosity: 3.4; melting point: 220°C; MFR measured in accordance with ASTM D1238 at 230°C and a load of 2.16 kg: 6.4 g / 10 min; terminal amino group concentration: 4.0 x 10 -5 eq / g)
[0144] (2) Acid-modified ethylene / α-olefin copolymer (B) Maleic anhydride-modified ethylene / 1-hexene copolymer (B-1): F3000 manufactured by Ube Maruzen Polyethylene Co., Ltd. (melting point: 115°C; MFR measured in accordance with ASTM D1238 at 230°C and a load of 2.16 kg: 8.5 g / 10 min; maleic anhydride modification rate: 1% by mass)
[0145] (3) Polyolefin (D) having no functional group: Linear low-density polyethylene (D-1): 1520F manufactured by Ube Maruzen Polyethylene Co., Ltd. (melting point: 114°C; MFR measured at 190°C and a load of 2.16 kg in accordance with ASTM D1238: 2 g / 10 min)
[0146] (4) Other raw materials Antioxidant: hindered phenol-based antioxidant (manufactured by BASF, Irganox (registered trademark) 1010) Compound (E): ethylene bisstearamide (manufactured by Kyoeisha Chemical Co., Ltd.) Compound (F) 1: magnesium stearate (manufactured by NOF Corporation, magnesium stearate) Compound (F) 2: calcium stearate (manufactured by NOF Corporation, calcium stearate)
[0147] Example 1 10.00% by mass of polyamide resin (A-1) as the first aliphatic polyamide resin (a1) was added with 2.50% by mass of maleic anhydride-modified ethylene / 1-hexene copolymer (B-1), and using a twin-screw kneader ZSK32McPlus (manufactured by Coperion Co., Ltd., screw diameter 32 mm), the cylinder temperature of the twin-screw kneader was 230 ° C., the screw rotation speed was 500 rpm, and the discharge rate was 75 kg / h. The first pellets were produced. Next, second pellets were produced using polyamide resin (A-2) as the second aliphatic polyamide resin (a2). Finally, 12.50% by mass of the first pellets, 87.28% by mass of the second pellets, 0.10% by mass of antioxidant, 0.06% by mass of compound (E), 0.03% by mass of compound (F) 1, and 0.03% by mass of compound (F) 2 were dry-blended to obtain a pellet mixture. The formulation of the pellet mixture of Example 1 is shown in Table 1.
[0148] Using the pellet mixture of Example 1, unstretched polyamide films a and b were prepared as follows.
[0149] Unstretched Polyamide Film a Using the pellet mixture of Example 1, an unstretched polyamide film a having a thickness of 50 μm was produced using a 40 mmφEx T-die film molding machine manufactured by Plastics Technology Research Institute Co., Ltd.
[0150] Unstretched Polyamide Film b Using the pellet mixture of Example 1, an unstretched polyamide film b having a thickness of 30 μm was produced using a 40 mmφEx T-die film molding machine manufactured by Plastics Technology Research Institute Co., Ltd.
[0151] Examples 2 and 5 and Comparative Examples 1, 2, 4 and 5 Pellet mixtures and polyamide films a to b of Examples 2 and 5 and Comparative Examples 1, 2, 4 and 5 were obtained in the same manner as in Example 1, except that the types and proportions of each component were changed as shown in Table 1.
[0152] Example 3 5.80% by mass of polyamide resin (A-1) as the first aliphatic polyamide resin (a1) was added with 2.50% by mass of maleic anhydride-modified ethylene / 1-hexene copolymer (B-1), and a twin-screw kneader ZSK32McPlus (manufactured by Coperion Co., Ltd., screw diameter 32 mm) was used, and the cylinder temperature of the twin-screw kneader was set to 230 ° C., the screw rotation speed was set to 500 rpm, and the discharge rate was set to 75 kg / h. The first pellets were then produced. Next, a second pellet was produced using polyamide resin (A-2) as the second aliphatic polyamide resin (a2). In addition, a third pellet was produced using linear low-density polyethylene (D-1) as the polyolefin (D) having no functional group. Finally, 8.30% by mass of the first pellets, 88.98% by mass of the second pellets, 2.50% by mass of the third pellets, 0.10% by mass of an antioxidant, 0.06% by mass of compound (E), 0.03% by mass of compound (F) 1, and 0.03% by mass of compound (F) 2 were dry-blended to obtain a pellet mixture. The composition of the pellet mixture of Example 3 is shown in Table 1.
[0153] Polyamide films a to b were obtained in the same manner as in Example 1, except that the pellet mixture of Example 3 was used.
[0154] Example 4 A pellet mixture and polyamide films a to b of Example 4 were obtained in the same manner as in Example 3, except that the proportions of the components were changed as shown in Table 1.
[0155] Comparative Example 3: Only pellets of polyamide resin (A-2) were used. 99.78% by mass of the pellets, 0.10% by mass of antioxidant, 0.06% by mass of compound (E), 0.03% by mass of compound (F) 1, and 0.03% by mass of compound (F) 2 were dry-blended to obtain a pellet mixture. The composition of the pellet mixture of Comparative Example 3 is shown in Table 1. The pellets used in Comparative Example 3 are shown in the second pellet column of Table 1.
[0156] Polyamide films a to b were obtained in the same manner as in Example 1, except that the pellet mixture of Comparative Example 3 was used.
[0157] Table 1 shows the formulations of Examples 1 to 5 and Comparative Examples 1 to 5 and various physical properties of the resulting polyamide resin compositions. In Table 1, the high-side and low-side melting peak temperatures refer to the top temperatures of the endothermic peaks observed in the ranges of 150 to 250°C and 70 to 120°C on the DSC curve, respectively. The high-side and low-side crystallization temperatures refer to the top temperatures of the exothermic peaks observed in the ranges of 120 to 200°C and 60 to 110°C on the DSC curve, respectively. "N.D." in the columns for the low-side melting peak temperature and the low-side crystallization temperature indicates that no peaks were detected.
[0158]
[0159] [Evaluation] The following properties were evaluated for each of the polyamide films produced in Examples 1 to 5 and Comparative Examples 1 to 5. The evaluation results are shown in Table 2.
[0160] 1. Resin pressure and resin temperature during film molding When producing unstretched polyamide film a, the resin pressure and resin temperature at the outlet of the T-die film molding machine were measured. It was determined that a resin pressure of 0.5 to 4.5 MPa indicated good moldability, and a resin pressure of 1.0 to 4.0 MPa indicated particularly excellent moldability. Keeping the resin pressure within the above ranges allows for increased film molding production speed and prevents resin leakage from the molding machine.
[0161] 2. Tensile Test After storing unstretched polyamide film a for one day at 23°C and 50% RH, the tensile strength, tensile elongation at break, and modulus of elasticity in the MD and TD directions were measured in the same environment at a tension speed of 300 mm / min in accordance with JIS K 7127. If the tensile strength at break was 80 MPa or more in the MD or TD direction, the film was judged to have excellent tensile strength. If the tensile elongation at break was 500% or more in the MD or TD direction, the film was judged to have excellent elongation. If the modulus of elasticity was 700 MPa or less in the MD or TD direction, the film was judged to have excellent flexibility.
[0162] 3. Haze Value (Haze Ratio) The haze value (haze ratio) of unstretched polyamide film a was measured in accordance with ASTM D-1003 using a Haze Meter manufactured by Nippon Denshoku Industries Co., Ltd. A haze ratio of 25% or less was determined to be practically acceptable, a haze ratio of 15% or less was determined to be excellent in transparency, and a haze ratio of 10% or less was determined to be particularly excellent in transparency.
[0163] The glossiness (gloss value) of unstretched polyamide film a was measured in accordance with ASTM D-523 using a digital variable-angle glossmeter manufactured by Suga Test Instruments Co., Ltd. A glossiness value of 50% or higher was considered to be acceptable for practical use, 80% or higher was considered to be excellent, and 100% or higher was considered to be particularly excellent.
[0164] 5. Puncture test After storing unstretched polyamide film a for one day at 23°C and 50% RH, the elongation at break and maximum point load were measured under the same conditions using a needle with a diameter of 1.0φ and a tip shape of 0.5R in accordance with JAS (P-1019). A maximum point load of 6.0 N or more was considered to be satisfactory for practical use, and a maximum point load of 8.0 N or more was considered to be particularly excellent in puncture strength.
[0165] 6. Coefficient of Friction After storing unstretched polyamide film a at 23°C and 50% RH for one day, the static and dynamic friction coefficients were measured five times under the same conditions in accordance with ASTM D-1894, and the average values were calculated. Note that the coefficient of friction for Comparative Example 3 was too high to measure. The pass criteria for the static and dynamic friction coefficients were each set to 1.0 or less.
[0166] 7. Film Gels The unstretched polyamide films b obtained in Examples 1 to 5 and Comparative Examples 1 to 5 were cut into A4 size pieces, and the number of film gels that had occurred was counted visually and rated according to the following criteria: ⊚: The number of gels that had occurred visually was less than 20; ◯: The number of gels that had occurred visually was 20 to 50; ×: The number of gels that had occurred visually was more than 50.
[0167] 8. Pinhole Resistance in Low-Temperature Environments The unstretched polyamide films b obtained in Examples 1 to 5 and Comparative Examples 1 to 5 were subjected to a 1,000-cycle bending test at 5°C in accordance with MIL-B-131C using a Gelbo Flex Tester with a thermostatic bath manufactured by Tester Sangyo Co., Ltd. After the bending test, the film was placed on a recording paper, and India ink was applied and allowed to penetrate the recording paper, and the number of recorded black dots was counted. The pinhole resistance was evaluated according to the following criteria: ⊚: The number of black dots was 70 or less / 0.03 m 2 ○: The number of black dots is more than 70 to 110 / 0.03 m 2 ×: The number of black dots is more than 110 / 0.03 m 2
[0168] 8. Recyclability Using the pellet mixtures obtained in Examples 1 to 5 and Comparative Examples 1 to 5, a 100 μm thick laminate film consisting of three layers laminated in this order: a 20 μm polyamide resin composition layer, a 10 μm adhesive layer, and a 70 μm polyethylene layer, was obtained using a three-type, three-layer co-extrusion air-cooled inflation molding machine (die diameter 100 mm) manufactured by Dr. Colin Co., Ltd. The adhesive layer was made of Admer (registered trademark) LF128 (acid-modified polyolefin resin) manufactured by Mitsui Chemicals, Inc., and the polyethylene layer was made of F022NH (low-density polyethylene resin) manufactured by Ube Maruzen Polyethylene Co., Ltd. The resulting laminate film was cut into flakes. Next, 20% by mass of the flakes were added to 80% by mass of F022NH (low-density polyethylene resin) manufactured by Ube Maruzen Polyethylene Co., Ltd., and the mixture was melt-kneaded using a twin-screw kneader ZSK32McPlus (manufactured by Coperion Co., Ltd., screw diameter 32 mm) at a cylinder temperature of 210°C, a screw rotation speed of 500 rpm, and a discharge rate of 75 kg / h to obtain recycled strands. The discharge stability, transparency, and surface roughness of the strands were visually confirmed, and the recyclability was evaluated according to the following criteria. Poor recyclability causes problems such as unstable strand discharge, lack of transparency, and rough surface. ⊚: Stable strand discharge, good transparency, no surface roughness, and excellent recyclability. ◯: Stable strand discharge, slight cloudiness observed but transparency maintained. Furthermore, the strand surface was only slightly rough, and recyclability was acceptable. x: Poor recyclability due to at least one of the following conditions: strand discharge is unstable, strands are cloudy and lack transparency, and strand surfaces are rough.
[0169] The evaluation results of the various films of Examples 1 to 5 and Comparative Examples 1 to 5 are shown in Table 2. In Table 2, "Not measurable" means that measurement was not possible.
[0170]
[0171] Table 2 shows that the compositions of Examples 1 to 5 produce films with excellent transparency, gloss, mechanical strength, coefficient of friction, and pinhole resistance without deterioration in appearance due to film gel, and also have excellent material recyclability. Furthermore, the compositions of Examples 1 to 5 contain 1 to 5 mass% of a functional group-containing ethylene / α-olefin copolymer (B) having 3 to 8 carbon atoms, and the DSC curves of the compositions have melting peaks in the range of 150 to 205°C. Therefore, excessive heating is not required during material recycling of waste laminate films containing at least a polyamide film layer and a polyolefin layer containing the composition, thereby suppressing deterioration in physical properties such as discoloration and thermal degradation of the polyolefin contained in the waste. A comparison of Examples 2 to 4 reveals that the compositions of Examples 3 and 4, which contain a non-functional polyolefin (D) in addition to the aliphatic polyamide resin (A) and copolymer (B), have significantly superior low-temperature pinhole resistance.
[0172] In Examples 1, 2, and 5, a film was produced by melt-kneading a pellet mixture containing first pellets containing a first aliphatic polyamide resin (a1) and a copolymer (B) in a predetermined ratio, and second pellets containing a second aliphatic polyamide resin (a2). In Examples 3 and 4, a film was produced by melt-kneading a pellet mixture containing, in addition to the first and second pellets, third pellets containing a polyolefin (D) having no functional groups. The use of such a pellet mixture not only allows the components to be uniformly mixed, suppresses the occurrence of film gels, but also results in low film-forming resin pressure and excellent formability.
[0173] Comparative Examples 1, 2, and 4, in which the content of the functional group-containing ethylene / α-olefin copolymer (B) having 3 to 8 carbon atoms exceeded 5% by mass, showed significant film gel generation and poor material recyclability. Comparative Examples 2 and 4 also showed poor film transparency and gloss. Comparative Example 3, in which the resin component was solely an aliphatic copolyamide, showed a high film friction coefficient and poor pinhole resistance in low-temperature environments and poor material recyclability. Comparative Example 5, in which the content of the functional group-containing ethylene / α-olefin copolymer (B) having 3 to 8 carbon atoms was 1 to 5% by mass but the aliphatic polyamide resin contained only an aliphatic homopolyamide, showed poor film elongation, flexibility, pinhole resistance in low-temperature environments, and poor material recyclability.
[0174] The film obtained from the polyamide resin composition of the present invention is particularly suitable for use in food packaging and is useful because it allows for excellent material recyclability of the film waste.
Claims
1. A polyamide resin composition comprising 88-99% by mass of an aliphatic polyamide resin (A), 1-5% by mass of a functional ethylene / α-olefin copolymer (B) having 3-8 carbon atoms, and 0-9% by mass of other components (C) relative to 100% by mass of the polyamide resin composition, wherein the ratio of the number of methylene groups to the number of amide groups in the aliphatic polyamide resin (A) is 3 or more and 11 or less, and the aliphatic polyamide resin (A) comprises 1-50% by mass of an aliphatic homopolyamide (A-1) and 50-99% by mass of an aliphatic copolyamide (A-2) relative to 100% by mass of the aliphatic polyamide resin (A), and the DSC curve of the polyamide resin composition when heated from 0°C to 280°C at a rate of 20°C / min in an air atmosphere has a melting peak in the range of 150-205°C, The polyamide resin composition has a number average molecular weight Mn of 50,000 to 60,000 as measured by GPC.
2. The polyamide resin composition according to claim 1, wherein the DSC curve further has a melting peak in the range of 70 to 120°C.
3. The polyamide resin composition according to claim 1 or 2, wherein the aliphatic copolyamide (A-2) is a copolymer selected from the group consisting of polyamide 6 / 66, polyamide 6 / 69, polyamide 6 / 11, polyamide 6 / 12, polyamide 6 / 66 / 11 and polyamide 6 / 66 / 12.
4. The polyamide resin composition according to claim 1 or 2, wherein the copolymer (B) is an ethylene / propylene copolymer, ethylene / 1-butene copolymer, ethylene / 1-hexene copolymer or ethylene / 1-octene copolymer having a group derived from maleic anhydride.
5. The polyamide resin composition according to claim 1 or 2, wherein the other component (C) comprises a polyolefin (D) having no functional group, and the content of the (D) component relative to 100% by mass of the polyamide resin composition is 2 to 8% by mass.
6. The polyamide resin composition according to claim 1 or 2, wherein the other component (C) comprises an antioxidant, and the content of the antioxidant relative to 100% by mass of the polyamide resin composition is 0.01 to 1% by mass.
7. The polyamide resin composition according to claim 1 or 2, wherein the other component (C) contains at least one compound (E) selected from the group consisting of methylene bis-stearamide, ethylene bis-stearamide, butylene bis-stearamide and hexamethylene bis-stearamide, and the content of compound (E) relative to 100% by mass of the polyamide resin composition is 0.01 to 1% by mass.
8. The polyamide resin composition according to claim 1 or 2, wherein the other component (C) contains at least one compound (F) selected from the group consisting of terminal-modified polyalkylene glycols, phosphates or phosphites, higher fatty acid monoesters, higher fatty acids, metal salts of higher fatty acids, higher fatty acid monoamides, N-substituted higher fatty acid monoamides, magnesium silicate, and substituted benzylidene sorbitols, and the content of compound (F) relative to 100% by mass of the polyamide resin composition is 0.01 to 1% by mass.
9. The polyamide resin composition according to claim 1 or 2, which is substantially free of silica.
10. A polyamide film comprising the polyamide resin composition according to claim 1 or 2.
11. A laminated film comprising at least three layers, in the order of a layer containing the polyamide resin composition according to claim 1 or 2, an adhesive layer and a polyolefin layer.
12. A laminated film comprising at least five layers, each of which is formed by laminating, in this order, an adhesive layer and a polyolefin layer on either side of a layer containing the polyamide resin composition according to claim 1 or 2.
13. The laminate film according to claim 11, wherein the layer containing the polyamide resin composition is a biaxially stretched layer.
14. The laminated film according to claim 11, which is for food packaging.
15. A pellet mixture comprising: first pellets comprising a first aliphatic polyamide resin (a1) and an ethylene / α-olefin copolymer having 3 to 8 carbon atoms (B) having a functional group; and second pellets comprising a second aliphatic polyamide resin (a2); wherein, in 100% by mass of the first pellets, the mixture comprises 60 to 90% by mass of the first aliphatic polyamide resin (a1), 10 to 40% by mass of the copolymer (B), and 0 to 9% by mass of other component (C), the aliphatic polyamide resin (a1) is an aliphatic homopolyamide, and the second aliphatic polyamide resin (a2) comprises, in relation to 100% by mass of the aliphatic polyamide resin (a2), 0 to 20% by mass of an aliphatic homopolyamide and 80 to 100% by mass of an aliphatic copolyamide, the content of the aliphatic homopolyamide is 1 to 50 mass% and the content of the aliphatic copolyamide is 50 to 99 mass% relative to 100 mass% in total of the first aliphatic polyamide resin (a1) and the second aliphatic polyamide resin (a2), and in each of the aliphatic polyamide resin (a1) and the aliphatic polyamide resin (a2), the ratio of the number of methylene groups to the number of amide groups is 3 or more and 11 or less, The pellet mixture contains, in 100 mass% of a kneaded product obtained by melt-kneading the pellet mixture, 88 to 99 mass% of a first aliphatic polyamide resin (a1) and a second aliphatic polyamide resin (a2), 1 to 5 mass% of the copolymer (B), and 0 to 9 mass% of other component (C), and the kneaded product has a melting peak in a range of 150 to 205°C in a DSC curve obtained by heating the kneaded product from 0°C to 280°C at a rate of 20°C / min in an air atmosphere, and the kneaded product has a number average molecular weight Mn of 50,000 to 60,000 as measured by GPC.
16. The pellet mixture according to claim 15, wherein the melting point of the copolymer (B) is 70 to 120°C.
17. The pellet mixture according to claim 15 or 16, further comprising third pellets containing a polyolefin (D) having no functional group, the content of the (D) component being 2 to 8 mass% relative to 100 mass% of the melt-kneaded mixture.
18. A first pellet for use in admixture with a second pellet in the preparation of a pellet mixture according to claim 15 or 16.
19. A second pellet for use in admixture with the first pellet in the preparation of the pellet mixture of claim 15 or 16.
Citation Information
Patent Citations
Polyamide resin composition
JP1992239559A
Polyamide resin composition and laminate made by using the same
JP1995003109A
Polyamide resin compound and polyamide film
JP2000109685A
Hydrogen tank liner material and hydrogen tank liner
JP2009191871A
Polyamide resin composition for film and polyamide film comprising the same
JP2011225870A