Resin composition, method for producing interlayer insulating film for rewiring layer, and photosensitive agent
The resin composition with a specific anion and cation addresses the challenge of low dielectric loss tangent and high resolution in interlayer insulating films by changing hydrophilicity and hydrophobicity upon exposure, improving the sensitivity and efficiency of film formation for electronic devices.
Patent Information
- Application Number
- PCT/JP2024/009318
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-11
- Publication Date
- 2024-10-03
AI Technical Summary
Interlayer insulating films for redistribution layers in electronic devices face challenges in reducing dielectric loss tangent and achieving high resolution, particularly with the increasing complexity and size of semiconductors and communication equipment.
A resin composition containing a specific anion and cation, represented by formulas (a1) and (b1), which undergoes photodecomposition to form a film with low dielectric loss tangent and high resolution, utilizing a photosensitizer for exposure and development.
The resin composition achieves a film with low dielectric loss tangent and excellent resolution by changing hydrophilicity and hydrophobicity upon exposure, avoiding the deterioration caused by radical polymerization, thus enhancing the sensitivity and efficiency of the film formation process.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Resin composition, method for producing interlayer insulating film for rewiring layer, and photosensitive agent
[0001] The present invention relates to a resin composition, a method for producing an interlayer insulating film for a rewiring layer, and a photosensitizer.
[0002] Resins such as polyimide and polybenzoxazole have excellent heat resistance and insulating properties and are therefore used in insulating films of electronic devices. Patent Document 1 describes a photosensitive resin composition containing a photobase generator having a specific structure and a polyimide precursor. Patent Document 2 describes a photosensitive resin composition containing a heterocycle-containing polymer precursor, a compound having a cation moiety with a specific structure and an anion moiety with radical initiation ability, and a radical polymerizable compound.
[0003] Japanese Patent Publication No. 2009-244745 Japanese Patent Publication No. 2016-27357
[0004] Recently, with the increasing frequency of communication devices, the increasing speed of computer devices, and the increasing size of semiconductors, interlayer insulating films for redistribution layers are required to have reduced transmission loss (dielectric loss tangent). Furthermore, excellent resolution is also required when forming an insulating pattern of the interlayer insulating film for redistribution layers. The present invention aims to provide a resin composition that can produce a film with a low dielectric loss tangent and excellent resolution, a method for producing an interlayer insulating film for redistribution layers using the resin composition, and a photosensitizer that can be used in the resin composition.
[0005] Examples of typical embodiments of the present invention are given below.
[0006] [1] A resin composition comprising an anion represented by the following formula (a1), a cation represented by the following formula (b1), and a resin:
[0007]
[0008] In formula (a1), R 1 ~R 3 R each independently represents a hydrogen atom, a halogen atom, a hydroxy group, an alkyl group, an alkenyl group, an alkynyl group, or an aryl group. 4 ~R 8R each independently represents a halogen atom, a monovalent organic group, or a hydrogen atom. 4 ~R 8 At least two of the groups may be bonded to form a ring. 9 ~R 12 R each independently represents a monovalent organic group or a hydrogen atom. 13 represents a monovalent organic group. 2 represents a single bond or a divalent linking group. p represents an integer of 1 to 5. q represents an integer of 0 to 4. R 10 If there are multiple R 10 may be the same or different. 11 and R 12 may be bonded to each other to form a ring. 11 If there are multiple R 11 may be the same or different, and at least two of them may be bonded to each other to form a ring. 12 If there are multiple R 12 may be the same or different, and at least two of them may be bonded to each other to form a ring. 13 If there are multiple R 13 may be the same or different, and at least two of them may be bonded to each other to form a ring. [2] The resin composition according to [1], wherein the anion is represented by the following formula (a2):
[0009]
[0010] In formula (a2), a to d each independently represent an integer of 0 to 5. 21 ~R 24 R each independently represents a halogen atom or a monovalent organic group. 21 If there are multiple R 21 may be the same or different, and at least two of them may be bonded to each other to form a ring. 22 If there are multiple R 22 may be the same or different, and at least two of them may be bonded to each other to form a ring. 23 If there are multiple R 23may be the same or different, and at least two of them may be bonded to each other to form a ring. 24 If there are multiple R 24 may be the same or different, and at least two of them may be bonded to each other to form a ring. [3] The resin composition according to [1] or [2], wherein the anion is represented by the following formula (a3):
[0011]
[0012] [4] The resin composition according to any one of [1] to [3], wherein the cation is represented by the following formula (b2):
[0013]
[0014] In formula (b2), R 9 ~R 12 each independently represents a monovalent organic group or a hydrogen atom. 2 represents a single bond or a divalent linking group. 11 and R 12 may be bonded to each other to form a ring. [5] Z in the above formula (b1) 2 is a single bond, —O—, —S—, —NR 14 -, *-OC(=O)-#, *-SC(=O)-#, *-NR 15 C(=O)-#, -OC(=O)O-, *-OC(=O)S-#, *-SC(=O)O-#, -SC(=O)S-, *-NR 16 C(=O)O-#, *-OC(=O)NR 17 -#, *-NR 18 C(=O)NR 19 -# or *-OS (=O) 2 -#, R 14 ~R 19 each independently represents a hydrogen atom, an alkyl group, or an aryl group, and * represents R 11 and R 12 represents the bonding position with the carbon atom to which it is bonded, and # represents R 10[6] The resin composition according to any one of [1] to [4], wherein the resin comprises at least one selected from the group consisting of polyimide, polyimide precursor, polybenzoxazole, and polybenzoxazole precursor. [7] The resin composition according to any one of [1] to [6], wherein the resin is used for organic solvent development. [8] The resin composition according to any one of [1] to [6], wherein the resin is used for aqueous solution development. [9] The resin composition according to any one of [1] to [8], wherein the resin is used for forming an interlayer insulating film for a redistribution layer.
[10] A method for producing an interlayer insulating film for a redistribution layer, comprising: a photosensitive film forming step of applying the resin composition according to any one of [1] to [9] onto a substrate to form a photosensitive film; an exposure step of exposing the photosensitive film to light to form an exposed film; and a pattern forming step of developing the exposed film with a developer to form an insulating pattern.
[11] The method for producing an interlayer insulating film for a redistribution layer according to
[10] , wherein the developer is an organic solvent.
[12] The method for producing an interlayer insulating film for a redistribution layer according to
[10] , wherein the developer is an aqueous solution.
[13] A photosensitizer represented by the following formula (z1):
[0015]
[0016] In formula (z1), R 9 ~R 12 each independently represents a monovalent organic group or a hydrogen atom. 2 represents a single bond or a divalent linking group. 11 and R 12 may be bonded to each other to form a ring.
[0017] According to the present invention, it is possible to provide a resin composition that can obtain a film with a low dielectric tangent and has excellent resolution, a method for producing an interlayer insulating film for a redistribution layer using the resin composition, and a photosensitizer that can be used in the resin composition.
[0018] The following describes the main embodiments of the present invention. However, the present invention is not limited to the explicitly described embodiments. In this specification, a numerical range expressed using the symbol "to" means a range that includes the numerical values before and after "to" as the lower and upper limits, respectively. In this specification, the term "process" refers not only to an independent process but also to a process that cannot be clearly distinguished from other processes as long as the process achieves its intended effect. In the description of a group (atomic group), a notation that does not specify whether it is substituted or unsubstituted encompasses both unsubstituted groups (atomic groups) and substituted groups (atomic groups). For example, the term "alkyl group" encompasses not only unsubstituted alkyl groups (unsubstituted alkyl groups) but also substituted alkyl groups (substituted alkyl groups). In this specification, unless otherwise specified, "exposure" includes not only exposure using light but also exposure using particle beams such as electron beams and ion beams. In addition, examples of light used for exposure include actinic rays or radiation such as the bright line spectrum of a mercury lamp, far ultraviolet light typified by excimer lasers, extreme ultraviolet light (EUV light), X-rays, and electron beams. As used herein, "(meth)acrylate" refers to either or both of "acrylate" and "methacrylate," "(meth)acrylic" refers to either or both of "acrylic" and "methacrylic," and "(meth)acryloyl" refers to either or both of "acryloyl" and "methacryloyl." In the structural formulae herein, Me represents a methyl group, Et represents an ethyl group, Bu represents a butyl group, and Ph represents a phenyl group. As used herein, the term "total solid content" refers to the total mass of all components of the composition excluding the solvent. Furthermore, as used herein, the term "solid content concentration" refers to the mass percentage of the components other than the solvent relative to the total mass of the composition. As used herein, the weight average molecular weight (Mw) and number average molecular weight (Mn) are values measured using gel permeation chromatography (GPC) and are defined as polystyrene equivalent values, unless otherwise specified.In this specification, the weight-average molecular weight (Mw) and number-average molecular weight (Mn) can be determined, for example, by using an HLC-8220GPC (manufactured by Tosoh Corporation) and guard columns HZ-L, TSKgel Super HZM-M, TSKgel Super HZ4000, TSKgel Super HZ3000, and TSKgel Super HZ2000 (all manufactured by Tosoh Corporation) connected in series. Unless otherwise specified, these molecular weights are measured using THF (tetrahydrofuran) as the eluent. However, when THF is not suitable as the eluent, for example, due to low solubility, NMP (N-methyl-2-pyrrolidone) can also be used. Furthermore, unless otherwise specified, detection in GPC measurement is assumed to be performed using a UV (ultraviolet) detector at a wavelength of 254 nm. In this specification, when the positional relationship of each layer constituting a laminate is described as "above" or "below," it is sufficient that another layer is above or below the reference layer among the multiple layers being considered. In other words, a third layer or element may be interposed between the reference layer and the other layer, and the reference layer and the other layer do not need to be in contact with each other. Unless otherwise specified, the direction in which layers are stacked on the substrate is referred to as "above." Alternatively, if a resin composition layer is present, the direction from the substrate to the resin composition layer is referred to as "above," and the opposite direction is referred to as "below." Note that such vertical directions are defined for convenience in this specification, and in actual embodiments, the "above" direction in this specification may differ from the vertically upward direction. In this specification, unless otherwise specified, the composition may contain two or more compounds corresponding to each component contained in the composition. Furthermore, unless otherwise specified, the content of each component in the composition means the total content of all compounds corresponding to that component. In this specification, unless otherwise specified, the temperature is 23° C., the atmospheric pressure is 101,325 Pa (1 atmosphere), and the relative humidity is 50% RH. In this specification, a combination of preferred embodiments is a more preferred embodiment.
[0019] [Resin Composition] The resin composition of the present invention is a resin composition containing an anion represented by the following formula (a1), a cation represented by the following formula (b1), and a resin.
[0020]
[0021] In formula (a1), R 1 ~R 3 R each independently represents a hydrogen atom, a halogen atom, a hydroxy group, an alkyl group, an alkenyl group, an alkynyl group, or an aryl group. 4 ~R 8 R each independently represents a halogen atom, a monovalent organic group, or a hydrogen atom. 4 ~R 8 At least two of the groups may be bonded to form a ring. 9 ~R 12 R each independently represents a monovalent organic group or a hydrogen atom. 13 represents a monovalent organic group. 2 represents a single bond or a divalent linking group. p represents an integer of 1 to 5. q represents an integer of 0 to 4. R 10 If there are multiple R 10 may be the same or different. 11 and R 12 may be bonded to each other to form a ring. 11 If there are multiple R 11 may be the same or different, and at least two of them may be bonded to each other to form a ring. 12 If there are multiple R 12 may be the same or different, and at least two of them may be bonded to each other to form a ring. 13 If there are multiple R 13 may be the same or different, and at least two of them may be bonded to each other to form a ring.
[0022] The resin composition of the present invention is preferably used to form a photosensitive film that is subjected to exposure and development, and is preferably used to form a film that is subjected to exposure and development using a developer containing an organic solvent or aqueous solution. The resin composition of the present invention can be used, for example, to form an insulating film for a semiconductor device, an interlayer insulating film for a redistribution layer, a stress buffer film, etc., and is preferably used to form an interlayer insulating film for a redistribution layer. The resin composition of the present invention may also be used to form a photosensitive film that is subjected to negative development or positive development. In the present invention, negative development refers to development in which non-exposed areas are removed by development in exposure and development, and positive development refers to development in which exposed areas are removed by development. As the exposure method, the developer, and the development method, for example, the exposure method described in the exposure step and the developer and development method described in the development step in the description of the method for producing a cured product described below can be used.
[0023] The resin composition of the present invention can produce a film with a low dielectric loss tangent. Furthermore, the resin composition of the present invention has excellent resolution. While the mechanism by which the above-described effects are achieved by the present invention is not clear, the inventors have hypothesized the following. However, the present invention is not limited by the hypothetical mechanism. When a film formed from the resin composition of the present invention is exposed to light, the anion represented by formula (a1) decomposes and releases electrons, and the cation represented by formula (b1) accepts these electrons to produce a decomposition product. The anion and cation before decomposition are ionic and hydrophilic compounds, whereas the decomposition product is a nonionic and hydrophobic compound. Therefore, the hydrophilicity and hydrophobicity of the film formed from the resin composition of the present invention change before and after exposure, resulting in a change in its solubility in a developer. It is believed that this mechanism results in a difference in dissolution rate in a developer between the exposed and unexposed areas of the film formed from the resin composition of the present invention, resulting in high resolution. Furthermore, in conventional methods that generate a difference in dissolution rate between exposed and unexposed areas in a developer depending on whether or not radical polymerization is performed, a resin having a radical polymerizable group and a crosslinker (radical polymerizable compound) are used, but these reaction products remain in the film and are thought to be a factor in the deterioration of the dielectric loss tangent. In contrast, when the resin composition of the present invention is used, as described above, a difference in dissolution rate between exposed and unexposed areas in a developer is generated by changing the hydrophilicity / hydrophobicity due to light acceptance / electron donor / electron acceptor using anions and cations. Therefore, no substances that cause the deterioration of the dielectric loss tangent are generated, and it is thought that the dielectric loss tangent can be reduced. Furthermore, as described above, in the resin composition of the present invention, a series of light acceptance / electron donor / electron acceptor phenomena occurs between anions and cations, which is thought to allow the reaction to proceed efficiently and improve sensitivity.
[0024] The components contained in the resin composition of the present invention will be described in detail below.
[0025] <Anion Represented by Formula (a1)> The resin composition of the present invention contains an anion represented by formula (a1) (also referred to as "specific anion").
[0026]
[0027] In formula (a1), R 1 ~R 3 R each independently represents a hydrogen atom, a halogen atom, a hydroxy group, an alkyl group, an alkenyl group, an alkynyl group, or an aryl group. 4 ~R 8 R each independently represents a halogen atom, a monovalent organic group, or a hydrogen atom. 4 ~R 8 At least two of these may be bonded to form a ring.
[0028] R in formula (a1) 1 ~R 3 The halogen atom represented by R in formula (a1) is preferably a fluorine atom, a chlorine atom, a bromine atom or an iodine atom, and more preferably a fluorine atom. 1 ~R 3 The alkyl group represented by may be linear or branched. The number of carbon atoms in the alkyl group is not particularly limited, and is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 6. The alkyl group may have a substituent. The alkyl group may also contain an ether bond in the chain. R in formula (a1) 1 ~R 3 The alkenyl group represented by may be linear or branched. The number of carbon atoms in the alkenyl group is not particularly limited, and is preferably 2 to 20, more preferably 2 to 10, and even more preferably 2 to 6. The alkenyl group may have a substituent. The alkenyl group may also contain an ether bond in the chain. R in formula (a1) 1 ~R 3 The alkynyl group represented by may be linear or branched. The number of carbon atoms in the alkynyl group is not particularly limited, and is preferably 2 to 20, more preferably 2 to 10, and even more preferably 2 to 6. The alkynyl group may have a substituent. The alkynyl group may also contain an ether bond in the chain. R in formula (a1) 1 ~R 3 The number of carbon atoms in the aryl group represented by is not particularly limited, and is, for example, preferably 6 to 20, more preferably 6 to 15, and even more preferably 6 to 10. The aryl group may have a substituent.
[0029] R in formula (a1) 1 ~R3 Preferably, each independently represents a halogen atom, a hydroxy group or an aryl group, more preferably an aryl group.
[0030] R in formula (a1) 4 ~R 8 The halogen atom represented by R in formula (a1) is preferably a fluorine atom, a chlorine atom, a bromine atom or an iodine atom, and more preferably a fluorine atom or a chlorine atom. 4 ~R 8 The number of carbon atoms in the monovalent organic group represented by is not particularly limited, and is, for example, preferably 1 to 30, more preferably 1 to 20, and even more preferably 1 to 10. The monovalent organic group is preferably, for example, an alkyl group, an alkenyl group, an alkynyl group, a cycloalkyl group, an aryl group, an alkoxy group, a cycloalkyloxy group, an aryloxy group, an acyl group, an acyloxy group, an alkylcarbonyloxy group, a cycloalkylcarbonyloxy group, an arylcarbonyloxy group, an alkylthio group, a cycloalkylthio group, an arylthio group, an alkylamino group, a cycloalkylamino group, an arylamino group, or a group formed by combining two or more of these. The monovalent organic group may have a substituent.
[0031] R in formula (a1) 4 ~R 8 At least two of R may be bonded to form a ring. 4 ~R 8 The ring formed by bonding at least two of these may be an aromatic ring or a non-aromatic ring.
[0032] R in formula (a1) 4 ~R 8 preferably represents a hydrogen atom, a halogen atom or an alkyl group, and more preferably represents a hydrogen atom.
[0033] The specific anion is preferably represented by the following formula (a2).
[0034]
[0035] In formula (a2), a to d each independently represent an integer of 0 to 5. 21 ~R 24R each independently represents a halogen atom or a monovalent organic group. 21 If there are multiple R 21 may be the same or different, and at least two of them may be bonded to each other to form a ring. 22 If there are multiple R 22 may be the same or different, and at least two of them may be bonded to each other to form a ring. 23 If there are multiple R 23 may be the same or different, and at least two of them may be bonded to each other to form a ring. 24 If there are multiple R 24 may be the same or different, and at least two of them may be bonded to each other to form a ring.
[0036] In formula (a2), a to d each independently preferably represent an integer of 0 to 4, more preferably an integer of 0 to 3, even more preferably an integer of 0 to 2, and particularly preferably 0 or 1.
[0037] R in formula (a2) 21 ~R 24 The halogen atom represented by R in formula (a2) is preferably a fluorine atom, a chlorine atom, a bromine atom or an iodine atom, and more preferably a fluorine atom or a chlorine atom. 21 ~R 24 The number of carbon atoms in the monovalent organic group represented by is not particularly limited, and is, for example, preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 5. The monovalent organic group is preferably, for example, an alkyl group, an alkenyl group, an alkynyl group, a cycloalkyl group, an aryl group, an alkoxy group, a cycloalkyloxy group, an aryloxy group, an acyl group, an acyloxy group, an alkylcarbonyloxy group, a cycloalkylcarbonyloxy group, an arylcarbonyloxy group, an alkylthio group, a cycloalkylthio group, an arylthio group, an alkylamino group, a cycloalkylamino group, an arylamino group, or a group formed by combining two or more of these. The monovalent organic group may have a substituent.
[0038] R in formula (a2) 21 ~R 24When a plurality of are present, they may be bonded to each other to form a ring, and the ring formed may be an aromatic ring or a non-aromatic ring.
[0039] R in formula (a2) 21 ~R 24 preferably represents a halogen atom or an alkyl group.
[0040] The specific anion is particularly preferably represented by the following formula (a3).
[0041]
[0042] The resin composition of the present invention may contain one type of specific anion or two or more types of specific anions.
[0043] <Cation Represented by Formula (b1)> The resin composition of the present invention contains a cation represented by formula (b1) (also referred to as a "specific cation").
[0044]
[0045] In formula (b1), R 9 ~R 12 R each independently represents a monovalent organic group or a hydrogen atom. 13 represents a monovalent organic group. 2 represents a single bond or a divalent linking group. p represents an integer of 1 to 5. q represents an integer of 0 to 4. R 10 If there are multiple R 10 may be the same or different. 11 and R 12 may be bonded to each other to form a ring. 11 If there are multiple R 11 may be the same or different, and at least two of them may be bonded to each other to form a ring. 12 If there are multiple R 12 may be the same or different, and at least two of them may be bonded to each other to form a ring. 13 If there are multiple R 13 may be the same or different, and at least two of them may be bonded to each other to form a ring.
[0046] R in formula (b1) 9 ~R13 The number of carbon atoms in the monovalent organic group represented by is not particularly limited, and is preferably 1 to 30, and more preferably 1 to 20. Examples of the monovalent organic group include an alkyl group, an alkenyl group, an alkynyl group, a cycloalkyl group, an aryl group, an alkoxy group, a cycloalkyloxy group, an aryloxy group, an acyl group, an acyloxy group, an alkylcarbonyloxy group, a cycloalkylcarbonyloxy group, an arylcarbonyloxy group, an alkylthio group, a cycloalkylthio group, an arylthio group, an alkylamino group, a cycloalkylamino group, an arylamino group, a heteroaryl group, or a group formed by combining two or more of these. The monovalent organic group may have a substituent.
[0047] R 9 ~R 13 The alkyl group represented by may be linear or branched. The number of carbon atoms in the alkyl group is not particularly limited, and is preferably 1 to 20, and may be 1 to 10, for example. The alkyl group may have a substituent. The alkyl group may also contain an ether bond in the chain. Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, a t-butyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, an n-tridecyl group, an n-tetradecyl group, and an n-pentadecyl group. R 9 ~R 13 The explanation, specific examples, and preferred ranges of the alkyl group contained in the alkoxy group, alkylcarbonyloxy group, alkylthio group, and alkylamino group represented by R are the same as those described above. 9 ~R 13 When the acyl group represented by R is an alkylcarbonyl group, the explanation, specific examples, and preferred ranges of the alkyl group contained in the alkylcarbonyl group are the same as those described above. 9 ~R 13 When the acyloxy group represented by the formula (I) is an alkylcarbonyloxy group, the explanation, specific examples and preferred ranges of the alkyl group contained in the alkylcarbonyloxy group are the same as those described above.
[0048] R 9 ~R13 The cycloalkyl group represented by may be monocyclic or polycyclic. The number of carbon atoms in the cycloalkyl group is not particularly limited, and is preferably 3 to 20, or may be 4 to 15, or may be 5 to 12. Examples of the cycloalkyl group include a cyclopentyl group, a 1-methylcyclopentyl group, a cyclohexyl group, an adamantyl group, a 1-ethyladamantyl group, a norbornyl group, a tetracyclodecanyl group, and a tetracyclododecanyl group. The cycloalkyl group may have a substituent. One of the methylene groups constituting the cycloalkane ring of the cycloalkyl group may be replaced with a heteroatom such as an oxygen atom, a carbonyl group, a sulfonyl group, or a group having a heteroatom such as an ester bond, or a vinylidene group. Furthermore, in the cycloalkyl group, one or more of the ethylene groups constituting the cycloalkane ring may be replaced with a vinylene group. 9 ~R 13 The explanation, specific examples, and preferred ranges of the cycloalkyl group contained in the cycloalkyloxy group, cycloalkylcarbonyloxy group, and cycloalkylthio group represented by R are the same as those described above. 9 ~R 13 When the acyl group represented by R is a cycloalkylcarbonyl group, the explanation, specific examples, and preferred ranges of the cycloalkyl group contained in the cycloalkylcarbonyl group are the same as those described above. 9 ~R 13 When the acyloxy group represented by the formula (I) is a cycloalkylcarbonyloxy group, the explanation, specific examples and preferred range of the cycloalkyl group contained in the cycloalkylcarbonyloxy group are the same as those described above.
[0049] R 9 ~R 13 The number of carbon atoms in the aryl group represented by is not particularly limited, and is preferably 6 to 20, and may be 6 to 15, for example. Examples of the aryl group include a phenyl group, a naphthyl group, an anthryl group, a fluorenyl group, a biphenyl group, and a pyrenyl group. The aryl group may have a substituent. A non-aromatic ring may be condensed with the aromatic ring of the aryl group. R 9 ~R 13The explanation, specific examples, and preferred ranges of the aryl group contained in the aryloxy group, arylcarbonyloxy group, and arylthio group represented by R are the same as those described above. 9 ~R 13 When the acyl group represented by R is an arylcarbonyl group, the explanation, specific examples, and preferred ranges of the aryl group contained in the arylcarbonyl group are the same as those described above. 9 ~R 13 When the acyloxy group represented by the formula (I) is an arylcarbonyloxy group, the explanation, specific examples and preferred ranges of the aryl group contained in the arylcarbonyloxy group are the same as those described above.
[0050] R 9 ~R 13 The alkenyl group represented by may be linear or branched. The number of carbon atoms in the alkenyl group is not particularly limited, and is preferably 2 to 20, and may be 2 to 10, for example. The alkenyl group may have a substituent. The alkenyl group may also contain an ether bond in the chain. Examples of the alkenyl group include a vinyl group and an allyl group. R 9 ~R 13 When the acyl group represented by R is an alkenylcarbonyl group, the explanation, specific examples, and preferred ranges of the alkenyl group contained in the alkenylcarbonyl group are the same as those described above. 9 ~R 13 When the acyloxy group represented by R is an alkenylcarbonyloxy group, the explanation, specific examples, and preferred ranges of the alkenyl group contained in the alkenylcarbonyloxy group are the same as those described above. 9 ~R 13 The alkynyl group represented by may be linear or branched. The number of carbon atoms in the alkynyl group is not particularly limited, and is preferably 2 to 20, and may be 2 to 10, for example. The alkynyl group may have a substituent. The alkynyl group may also contain an ether bond in the chain. Examples of the alkynyl group include an ethynyl group and a prop-2-yn-1-yl group. R 9 ~R 13When the acyl group represented by R is an alkynylcarbonyl group, the explanation, specific examples, and preferred ranges of the alkynyl group contained in the alkynylcarbonyl group are the same as those described above. 9 ~R 13 When the acyloxy group represented by the formula (I) is an alkynylcarbonyloxy group, the explanation, specific examples and preferred ranges of the alkynyl group contained in the alkynylcarbonyloxy group are the same as those described above.
[0051] R 9 ~R 13 The alkylamino group represented by may be a monoalkylamino group or a dialkylamino group. The explanation, specific examples, and preferred ranges for the alkyl group contained in the alkylamino group are the same as those described above. The monoalkylamino group may have a substituent other than the alkyl group. Examples of the substituent other than the alkyl group include a cycloalkyl group and an aryl group, and the explanation, specific examples, and preferred ranges for each are the same as those described above. R 9 ~R 13 The cycloalkylamino group represented by may be a monocycloalkylamino group or a dicycloalkylamino group. The explanation, specific examples, and preferred ranges for the cycloalkyl group contained in the cycloalkylamino group are the same as those described above. The monocycloalkylamino group may have a substituent other than the cycloalkyl group. Examples of the substituent other than the cycloalkyl group include an alkyl group and an aryl group, and the explanation, specific examples, and preferred ranges for each are the same as those described above. R 9 ~R 13 The arylamino group represented by may be a monoarylamino group or a diarylamino group. The explanation, specific examples, and preferred ranges for the aryl group contained in the arylamino group are the same as those described above. The monoarylamino group may have a substituent other than the aryl group. Examples of the substituent other than the aryl group include an alkyl group and a cycloalkyl group, and the explanation, specific examples, and preferred ranges for each are the same as those described above.
[0052] R 9 ~R 13The number of carbon atoms in the heteroaryl group represented by is not particularly limited, and is preferably 2 to 20, and may be 3 to 15, for example. The heteroaryl group preferably contains at least one heteroatom selected from the group consisting of an oxygen atom, a sulfur atom, and a nitrogen atom. Examples of heteroaryl groups include a pyrrolyl group, a furanyl group, a thiophenyl group, an indolyl group, a benzofuranyl group, a benzothiophenyl group, and a carbazolyl group. The heteroaryl group may have a substituent. A non-aromatic ring may be fused to the aromatic ring of the heteroaryl group.
[0053] R in formula (b1) 9 The monovalent organic group represented by is preferably an alkyl group. The alkyl group may be linear or branched. The number of carbon atoms in the alkyl group is not particularly limited, and is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 6. The alkyl group may have a substituent. Furthermore, the alkyl group may contain an ether bond in the chain.
[0054] R in formula (b1) 9 preferably represents a hydrogen atom or an alkyl group, and more preferably represents an alkyl group.
[0055] R in formula (b1) 10 R in formula (b1) preferably represents a monovalent organic group. 10 The monovalent organic group represented by R is preferably an alkyl group, an aryl group, or an acyl group. 10 The number of carbon atoms in the alkyl group represented by is not particularly limited, and is preferably 1 to 20, and more preferably 1 to 15, for example. The alkyl group may be linear or branched. The alkyl group may also contain an ether bond in the chain. The alkyl group may have a substituent. There is no particular limit to the substituent that the alkyl group may have, but an aryl group is preferred. As the aryl group, for example, an aryl group having 6 to 20 carbon atoms is preferred, and examples thereof include a phenyl group and a fluorenyl group. The aryl group may further have a substituent. R 10The number of carbon atoms in the aryl group represented by is not particularly limited, and is preferably 6 to 30, and more preferably 6 to 20. The aryl group may have a substituent. The aryl group is preferably a phenyl group, a naphthyl group, or an anthryl group. 10 The number of carbon atoms in the acyl group represented by is not particularly limited, and is, for example, preferably 2 to 20, more preferably 2 to 15. The acyl group may be an aromatic acyl group or an aliphatic acyl group. The acyl group may have a substituent.
[0056] R in formula (b1) 11 and R 12 The monovalent organic group represented by R is preferably an alkyl group. 11 and R 12 The number of carbon atoms in the alkyl group represented by is not particularly limited, and is, for example, preferably 1 to 20, more preferably 1 to 15. The alkyl group may be linear or branched. The alkyl group may have a substituent. Furthermore, the alkyl group may contain an ether bond in the chain.
[0057] R in formula (b1) 11 and R 12 preferably represents a hydrogen atom or an alkyl group, and more preferably represents a hydrogen atom.
[0058] R in formula (b1) 13 The monovalent organic group represented by R is preferably an alkyl group, an aryl group, or an alkenyl group. 13 The number of carbon atoms in the alkyl group represented by is not particularly limited, and is preferably 1 to 20, more preferably 1 to 15, for example. The alkyl group may be linear or branched. The alkyl group may have a substituent. The alkyl group may also contain an ether bond in the chain. R 13 The number of carbon atoms in the aryl group represented by is not particularly limited, and is preferably 6 to 30, and more preferably 6 to 20. The aryl group may have a substituent. The aryl group is preferably a phenyl group, a naphthyl group, or an anthryl group. 13 The number of carbon atoms in the alkenyl group represented by is not particularly limited, and is, for example, preferably 2 to 20, more preferably 2 to 15. The alkenyl group may be linear or branched. The alkenyl group may have a substituent.
[0059] R 13 If there are multiple R 13 may be bonded to each other to form a ring. The ring formed may be an aromatic ring or a non-aromatic ring, but is preferably an aromatic ring, and more preferably a benzene ring.
[0060] Z in formula (b1) 2 The divalent linking group represented by is not particularly limited, and examples thereof include —O—, —S—, and —NR 14 -, *-OC(=O)-#, *-SC(=O)-#, *-NR 15 C(=O)-#, -OC(=O)O-, *-OC(=O)S-#, *-SC(=O)O-#, -SC(=O)S-, *-NR 16 C(=O)O-#, *-OC(=O)NR 17 -#, *-NR 18 C(=O)NR 19 -# and *-OS (=O) 2 -# is preferred. 14 ~R 19 each independently represents a hydrogen atom, an alkyl group, or an aryl group, and * represents R 11 and R 12 represents the bonding position with the carbon atom to which it is bonded, and # represents R 10 represents the bonding position with 14 ~R 19 The number of carbon atoms in the alkyl group represented by is not particularly limited, and is preferably 1 to 20, more preferably 1 to 15, for example. The alkyl group may be linear or branched. The alkyl group may have a substituent. The alkyl group may also contain an ether bond in the chain. R 14 ~R 19 The number of carbon atoms in the aryl group represented by R is not particularly limited, and is preferably 6 to 30, and more preferably 6 to 20. The aryl group may have a substituent. 14 ~R 19 is R in formula (b1) 10 may be bonded to form a ring.
[0061] In formula (b1), p preferably represents an integer of 1 to 4, more preferably an integer of 1 to 3, even more preferably 1 or 2, and particularly preferably 1.
[0062] In formula (b1), q preferably represents an integer of 0 to 3, more preferably an integer of 0 to 2, even more preferably 0 or 1, and particularly preferably 0. The sum of p and q in formula (b1) is an integer of 1 to 5.
[0063] The specific cation is preferably represented by the following formula (b2).
[0064]
[0065] In formula (b2), R 9 ~R 12 each independently represents a monovalent organic group or a hydrogen atom. 2 represents a single bond or a divalent linking group. 11 and R 12 may be bonded to each other to form a ring.
[0066] R in formula (b2) 9 ~R 12 , and Z 2 The explanation, specific examples and preferred ranges of R in formula (b1) are 9 ~R 12 , and Z 2 is the same as
[0067] The resin composition of the present invention may contain one type of specific cation or two or more types of specific cations.
[0068] The mass ratio of the specific anion to the specific cation contained in the resin composition of the present invention, specific anion:specific cation, is preferably 0.5:1 to 1:0.5, more preferably 0.7:1 to 1:0.7, and particularly preferably 0.8:1 to 1:0.8.
[0069] When preparing the resin composition of the present invention, the specific anion and the specific cation may be contained in the same compound or in different compounds. For example, the specific anion and the specific cation may be contained in the resin composition by using a compound containing the specific anion and the specific cation. Alternatively, the specific anion and the specific cation may be contained in the resin composition by using a compound containing the specific anion and a cation other than the specific cation, or a compound containing an anion other than the specific anion and the specific cation. As described above, the specific anion releases electrons upon exposure and decomposes, so the compound containing the specific anion can be referred to as a photosensitizer. The specific anion and the specific cation can be synthesized by known methods.
[0070] [Content] The total amount of the specific anion and the specific cation contained in the resin composition of the present invention is not particularly limited, but is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 1% by mass or more, particularly preferably 5% by mass or more, and most preferably 10% by mass or more, based on the total solid content of the resin composition. Furthermore, the total amount of the specific anion and the specific cation contained in the resin composition of the present invention is preferably 70% by mass or less, more preferably 50% by mass or less, even more preferably 40% by mass or less, particularly preferably 30% by mass or less, and most preferably 20% by mass or less, based on the total solid content of the resin composition. The resin composition of the present invention may contain only one type of specific anion and one type of specific cation, or two or more types. When two or more types are contained, the total amount of all specific anions and specific cations is preferably within the above range.
[0071] <Resin> The resin composition of the present invention contains a resin. The resin is not particularly limited, but is preferably at least one resin (also referred to as a "specific resin") selected from the group consisting of cyclized resins and their precursors. The cyclized resin is preferably a resin containing an imide ring structure or an oxazole ring structure in its main chain structure. In the present invention, the term "main chain" refers to the relatively longest bonded chain in a resin molecule, and the term "side chain" refers to any other bonded chain. Examples of cyclized resins include polyimide, polybenzoxazole, and polyamideimide. A precursor of a cyclized resin refers to a resin whose chemical structure changes upon external stimulation to become a cyclized resin. Resins whose chemical structure changes upon heating to become a cyclized resin are preferred, and resins whose ring structure is formed by a ring-closing reaction upon heating to become a cyclized resin are more preferred. Examples of precursors of cyclized resins include polyimide precursors, polybenzoxazole precursors, and polyamideimide precursors. The resin composition of the present invention preferably contains at least one selected from the group consisting of polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, polyamideimide, and polyamideimide precursor, more preferably at least one selected from the group consisting of polyimide, polyimide precursor, polybenzoxazole, and polybenzoxazole precursor, and even more preferably at least one selected from the group consisting of polyimide and polyimide precursor. The resin may have a polymerizable group (e.g., a radically polymerizable group). The resin may also have a polarity conversion group such as an acid-decomposable group. When the resin has an acid-decomposable group, the resin composition preferably contains a photoacid generator. From such a resin composition, for example, a chemically amplified positive-type photosensitive film or negative-type photosensitive film is formed.
[0072] [Polyimide Precursor] The type of polyimide precursor is not particularly limited, but it is preferable that the polyimide precursor contains a repeating unit represented by the following formula (2).
[0073]
[0074] In formula (2), A 1 and A 2are each independently an oxygen atom or —NR z represents -, and R 111 represents a divalent organic group, and R 115 represents a tetravalent organic group, R 113 and R 114 each independently represents a hydrogen atom or a monovalent organic group; R z represents a hydrogen atom or a monovalent organic group.
[0075] A in formula (2) 1 and A 2 are each independently an oxygen atom or —NR z - represents. z represents a hydrogen atom or a monovalent organic group, and is preferably a hydrogen atom. 1 and A 2 is preferably an oxygen atom or —NH—, more preferably an oxygen atom. 111 represents a divalent organic group. Examples of the divalent organic group include groups containing a linear or branched aliphatic group, a cyclic aliphatic group, and an aromatic group, and a linear or branched aliphatic group having 2 to 20 carbon atoms, a cyclic aliphatic group having 3 to 20 carbon atoms, an aromatic group having 3 to 20 carbon atoms, or a group consisting of a combination thereof is preferred, and a group containing an aromatic group having 6 to 20 carbon atoms is more preferred. The linear or branched aliphatic group may have a hydrocarbon group in the chain substituted with a group containing a heteroatom, and the cyclic aliphatic group and aromatic group may have a hydrocarbon group in the ring substituted with a group containing a heteroatom. R in formula (2) 111 Examples of the group include groups represented by -Ar- and -Ar-L-Ar-, and the group represented by -Ar-L-Ar- is preferred, where each Ar is independently an aromatic group, L is a single bond, an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom, -O-, -CO-, -S-, or -SO 2 - or -NHCO-, or a group consisting of a combination of two or more of the above. The preferred ranges for these are as described above.
[0076] R 111is preferably derived from a diamine. Examples of diamines used in the production of the polyimide precursor include linear or branched aliphatic, cyclic aliphatic, or aromatic diamines. Only one type of diamine may be used, or two or more types may be used. Specifically, R 111 is preferably a diamine containing a linear or branched aliphatic group having 2 to 20 carbon atoms, a cyclic aliphatic group having 3 to 20 carbon atoms, an aromatic group having 3 to 20 carbon atoms, or a group consisting of a combination thereof, and more preferably a diamine containing an aromatic group having 6 to 20 carbon atoms. The linear or branched aliphatic group may have a hydrocarbon group in the chain substituted with a group containing a heteroatom, and the cyclic aliphatic group and aromatic group may have a hydrocarbon group in the ring substituted with a group containing a heteroatom. Examples of groups containing an aromatic group include the following.
[0077]
[0078] In the formula, A represents a single bond or a divalent linking group, and is selected from the group consisting of a single bond, an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom, —O—, —C(═O)—, —S—, and —SO 2 -, -NHCO-, or a group selected from a combination thereof, and is preferably a single bond, an alkylene group having 1 to 3 carbon atoms which may be substituted with a fluorine atom, -O-, -C(=O)-, -S-, or -SO 2 - is more preferably a group selected from -CH 2 -, -O-, -S-, -SO 2 -, -C(CF 3 ) 2 - or -C(CH 3 ) 2 In the formula, * represents a bonding site to another structure.
[0079] Specific examples of diamines include 1,2-diaminoethane, 1,2-diaminopropane, 1,3-diaminopropane, 1,4-diaminobutane, and 1,6-diaminohexane; 1,2- or 1,3-diaminocyclopentane, 1,2-, 1,3-, or 1,4-diaminocyclohexane, 1,2-, 1,3-, or 1,4-bis(aminomethyl)cyclohexane, bis-(4-aminocyclohexyl)methane, bis-(3-aminocyclohexyl)methane, 4,4'-diamino-3,3'-dimethylcyclohexylmethane, and isophoronediamine; m- or p-phenylenediamine, diaminotoluene, 4,4'- or 3,3'-diaminobiphenyl, 4,4'-diaminodiphenyl ether, 3,3-diaminodiphenyl ether, 4,4'- or 3,3'-diaminodiphenylmethane, 4,4'- or 3,3'-diaminodiphenyl sulfone, 4,4'- or 3,3'-diaminodiphenyl sulfide, 4,4'- or 3,3'-diaminobenzophenone, 3 ,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis(3-hydroxy-4-aminophenyl)propane, 2,2-bis(3-hydroxy-4-aminophenyl)hexafluoropropane parafluoropropane, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, bis(3-amino-4-hydroxyphenyl)sulfone, bis(4-amino-3-hydroxyphenyl)sulfone, 4,4'-diaminoparaterphenyl, 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(2-aminophenoxy)phenyl]sulfone, 1,4-bis(4-aminophenoxy)benzene, 9,10-bis(4-aminophenyl)anthracene, 3,3'-dimethyl-4,4'-diaminodiphenylsulfone, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenyl)benzene, 3,3'-diethyl-4,4'-diaminodiphenylmethane, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 4,4'-diaminooctafluorobiphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 9,9-bis(4-aminophenyl)-10-hydroanthracene, 3,3',4,4'-tetraaminobiphenyl, 3,3',4,4'-tetraaminodiphenyl ether fluorene, 1,4-diaminoanthraquinone, 1,5-diaminoanthraquinone, 3,3-dihydroxy-4,4'-diaminobiphenyl, 9,9'-bis(4-aminophenyl)fluorene, 4,4'-dimethyl-3,3'-diaminodiphenyl sulfone, 3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, 2,4- and 2,5-diaminocumene, 2,5-dimethyl-p-phenylenediamine, acetoguanamine, 2,3,5,6-tetramethyl-p-phenylenediamine, 2,4,6-trimethyl-m-phenylenediamine bis(3-aminopropyl)tetramethyldisiloxane, bis(p-aminophenyl)octamethylpentasiloxane, 2,7-diaminofluorene, 2,5-diaminopyridine, 1,2-bis(4-aminophenyl)ethane, diaminobenzanilide, esters of diaminobenzoic acid, 1,5-diaminonaphthalene, diaminobenzotrifluoride, 1,3-bis(4-aminophenyl)hexafluoropropane, 1,4-bis(4-aminophenyl)octafluorobutane, 1,5-bis(4-aminophenyl)decafluoropentane, 1,7-bis(4-aminophenyl)tetradecafluoroheptane, 2,2-bis[4-(3-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis[4-(2-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)-3,5-dimethylphenyl]hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)-3,5-bis(trifluoromethyl)phenyl]hexafluoropropane, p-bis(4-amino-2-trifluoromethylphenoxy)benzene, 4,At least one diamine selected from 4'-bis(4-amino-2-trifluoromethylphenoxy)biphenyl, 4,4'-bis(4-amino-3-trifluoromethylphenoxy)biphenyl, 4,4'-bis(4-amino-2-trifluoromethylphenoxy)diphenyl sulfone, 4,4'-bis(3-amino-5-trifluoromethylphenoxy)diphenyl sulfone, 2,2-bis[4-(4-amino-3-trifluoromethylphenoxy)phenyl]hexafluoropropane, 3,3',5,5'-tetramethyl-4,4'-diaminobiphenyl, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 2,2',5,5',6,6'-hexafluorotolidine, and 4,4'-diaminoquaterphenyl can be mentioned.
[0080] Also preferred are the diamines (DA-1) to (DA-18) described in paragraphs 0030 to 0031 of WO 2017 / 038598.
[0081] Also preferably used are diamines having two or more alkylene glycol units in the main chain described in paragraphs 0032 to 0034 of WO 2017 / 038598.
[0082] R 111 is preferably represented by -Ar-L-Ar- from the viewpoint of flexibility of the resulting organic film, wherein each Ar is independently an aromatic group, and L is an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom, -O-, -CO-, -S-, or -SO 2 Ar is preferably a phenylene group, and L is preferably an aliphatic hydrocarbon group having 1 or 2 carbon atoms which may be substituted with a fluorine atom, -O-, -CO-, -S-, or -SO 2 The aliphatic hydrocarbon group here is preferably an alkylene group.
[0083] Also, R 111 is preferably a divalent organic group represented by the following formula (51) or formula (61) from the viewpoint of i-line transmittance. In particular, from the viewpoint of i-line transmittance and ease of availability, it is more preferably a divalent organic group represented by formula (61).
[0084]
[0085] In formula (51), R 50 ~R 57 are each independently a hydrogen atom, a fluorine atom, or a monovalent organic group, and R 50 ~R 57 At least one of R is a fluorine atom, a methyl group, or a trifluoromethyl group, and * each independently represents a bonding site with the nitrogen atom in formula (2). 50 ~R 57 Examples of the monovalent organic group include an unsubstituted alkyl group having 1 to 10 carbon atoms (preferably 1 to 6 carbon atoms) and a fluorinated alkyl group having 1 to 10 carbon atoms (preferably 1 to 6 carbon atoms).
[0086]
[0087] In formula (61), R 58 and R 59 are each independently a fluorine atom, a methyl group, or a trifluoromethyl group, and * each independently represents a bonding site with the nitrogen atom in formula (2). Examples of diamines that give the structure of formula (51) or formula (61) include 2,2'-dimethylbenzidine, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,2'-bis(fluoro)-4,4'-diaminobiphenyl, and 4,4'-diaminooctafluorobiphenyl. These may be used alone or in combination of two or more.
[0088] R in formula (2) 115 represents a tetravalent organic group. As the tetravalent organic group, a tetravalent organic group containing an aromatic ring is preferred, and a group represented by the following formula (5) or formula (6) is more preferred. In formula (5) or formula (6), * each independently represents a bonding site to another structure.
[0089]
[0090] In formula (5), R 112 represents a single bond or a divalent linking group, and is a single bond, or an aliphatic hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a fluorine atom, -O-, -CO-, -S-, -SO 2-, -NHCO-, and a group selected from a combination thereof are preferred, and a single bond, an alkylene group having 1 to 3 carbon atoms which may be substituted with a fluorine atom, -O-, -CO-, -S-, and -SO 2 - is more preferably a group selected from -CH 2 -, -C(CF 3 ) 2 -, -C(CH 3 ) 2 -, -O-, -CO-, -S- and -SO 2 It is more preferably a divalent group selected from the group consisting of -.
[0091] R 115 Specifically, R may be a tetracarboxylic acid residue remaining after removal of the anhydride group from a tetracarboxylic dianhydride. 115 The tetracarboxylic acid dianhydride may contain only one kind or two or more kinds of tetracarboxylic acid dianhydride residues as a structure corresponding to the formula (I). The tetracarboxylic acid dianhydride is preferably represented by the following formula (O).
[0092]
[0093] In formula (O), R 115 represents a tetravalent organic group. 115 The preferred range of R in formula (2) is 115 The same applies to the preferred range.
[0094] Specific examples of tetracarboxylic dianhydrides include pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfidetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-diphenylmethanetetracarboxylic dianhydride, 2,2 2,3,3',4'-diphenylmethanetetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-benzophenonetetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,4,5,7-naphthalenetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(2, 1,3-diphenylhexafluoropropane-3,3,4,4-tetracarboxylic dianhydride, 1,4,5,6-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-diphenyltetracarboxylic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 1,2,4,5-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 1,8,9,10-phenanthrenetetracarboxylic dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,2,3,4-benzenetetracarboxylic dianhydride, and alkyl and alkoxy derivatives having 1 to 6 carbon atoms thereof.
[0095] Further, tetracarboxylic dianhydrides (DAA-1) to (DAA-5) described in paragraph 0038 of WO 2017 / 038598 are also preferred examples.
[0096] In formula (2), R 111 and R 115 At least one of R may have an OH group. 111Examples of the amino acid residue include residues of bisaminophenol derivatives.
[0097] R in formula (2) 113 and R 114 each independently represents a hydrogen atom or a monovalent organic group. The monovalent organic group preferably contains a linear or branched alkyl group, a cyclic alkyl group, an aromatic group, or a polyalkyleneoxy group. 113 and R 114 At least one of R may contain a polymerizable group, or both may contain a polymerizable group. 113 and R 114 At least one of the groups may contain two or more polymerizable groups. The polymerizable group may be a group capable of undergoing a crosslinking reaction by the action of heat, radicals, or the like, or may be a radically polymerizable group. Specific examples of the polymerizable group include a group having an ethylenically unsaturated bond, an alkoxymethyl group, a hydroxymethyl group, an acyloxymethyl group, an epoxy group, an oxetanyl group, a benzoxazolyl group, a blocked isocyanate group, and an amino group. The radically polymerizable group contained in the polyimide precursor is preferably a group having an ethylenically unsaturated bond. Examples of the group having an ethylenically unsaturated bond include a vinyl group, an allyl group, an isoallyl group, a 2-methylallyl group, a group having an aromatic ring directly bonded to a vinyl group (e.g., a vinylphenyl group), a (meth)acrylamide group, a (meth)acryloyloxy group, and a group represented by the following formula (III):
[0098]
[0099] In formula (III), R 200 represents a hydrogen atom, a methyl group, an ethyl group, or a methylol group, and is preferably a hydrogen atom or a methyl group. In formula (III), * represents a bonding site with another structure. In formula (III), R 201 represents an alkylene group having 2 to 12 carbon atoms, —CH 2 CH(OH)CH 2 -, a cycloalkylene group or a polyalkyleneoxy group. 201Examples of the alkylene group include an ethylene group, a propylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, an octamethylene group, and a dodecamethylene group; a 1,2-butanediyl group, a 1,3-butanediyl group; a —CH 2 CH(OH)CH 2 alkylene groups such as ethylene and propylene; 2 CH(OH)CH 2More preferred are alkylene groups such as ethylene and propylene, or polyalkyleneoxy groups. In the present invention, a polyalkyleneoxy group refers to a group in which two or more alkyleneoxy groups are directly bonded. The alkylene groups in the multiple alkyleneoxy groups contained in the polyalkyleneoxy group may be the same or different. When a polyalkyleneoxy group contains multiple alkyleneoxy groups with different alkylene groups, the arrangement of the alkyleneoxy groups in the polyalkyleneoxy group may be a random arrangement, a block arrangement, or an arrangement having an alternating pattern. The number of carbon atoms in the alkylene group (including the number of carbon atoms in the substituent if the alkylene group has a substituent) is preferably 2 or more, more preferably 2 to 10, more preferably 2 to 6, even more preferably 2 to 5, even more preferably 2 to 4, even more preferably 2 or 3, and particularly preferably 2. The alkylene group may also have a substituent. Preferred substituents include alkyl groups, aryl groups, and halogen atoms. The number of alkyleneoxy groups contained in the polyalkyleneoxy group (the number of repeating polyalkyleneoxy groups) is preferably 2 to 20, more preferably 2 to 10, and even more preferably 2 to 6. From the viewpoint of solvent solubility and solvent resistance, the polyalkyleneoxy group is preferably a polyethyleneoxy group, a polypropyleneoxy group, a polytrimethyleneoxy group, a polytetramethyleneoxy group, or a group in which multiple ethyleneoxy groups and multiple propyleneoxy groups are bonded, more preferably a polyethyleneoxy group or a polypropyleneoxy group, and even more preferably a polyethyleneoxy group. In the group in which multiple ethyleneoxy groups and multiple propyleneoxy groups are bonded, the ethyleneoxy groups and propyleneoxy groups may be arranged randomly, in blocks, or in an alternating pattern. The preferred embodiments of the number of repeating ethyleneoxy groups and the like in these groups are as described above.
[0100] In formula (2), R 113is a hydrogen atom, or R 114 When is a hydrogen atom, the polyimide precursor may form a counter salt with a tertiary amine compound having an ethylenically unsaturated bond. An example of such a tertiary amine compound having an ethylenically unsaturated bond is N,N-dimethylaminopropyl methacrylate.
[0101] In formula (2), R 113 and R 114 At least one of the groups may be a polarity conversion group such as an acid-decomposable group. The acid-decomposable group is not particularly limited as long as it is decomposed by the action of an acid to generate an alkali-soluble group such as a phenolic hydroxy group or a carboxy group. Preferred examples include an acetal group, a ketal group, a silyl group, a silyl ether group, and a tertiary alkyl ester group. From the viewpoint of exposure sensitivity, an acetal group or a ketal group is more preferred. Specific examples of the acid-decomposable group include a tert-butoxycarbonyl group, an isopropoxycarbonyl group, a tetrahydropyranyl group, a tetrahydrofuranyl group, an ethoxyethyl group, a methoxyethyl group, an ethoxymethyl group, a trimethylsilyl group, a tert-butoxycarbonylmethyl group, and a trimethylsilyl ether group. From the viewpoint of exposure sensitivity, an ethoxyethyl group or a tetrahydrofuranyl group is preferred.
[0102] The polyimide precursor preferably contains fluorine atoms in its structure. The fluorine atom content in the polyimide precursor is preferably 10% by mass or more and 20% by mass or less.
[0103] Furthermore, for the purpose of improving adhesion to a substrate, the polyimide precursor may be copolymerized with an aliphatic group having a siloxane structure. Specific examples include embodiments using bis(3-aminopropyl)tetramethyldisiloxane, bis(p-aminophenyl)octamethylpentasiloxane, or the like as a diamine.
[0104] The repeating unit represented by formula (2) is preferably a repeating unit represented by formula (2-A). That is, it is preferable that at least one of the polyimide precursors used in the present invention is a precursor having a repeating unit represented by formula (2-A). When the polyimide precursor contains a repeating unit represented by formula (2-A), it becomes possible to further widen the width of the exposure latitude. Formula (2-A)
[0105]
[0106] In formula (2-A), A 1 and A 2 represents an oxygen atom, R 111 and R 112 each independently represents a divalent organic group; R 113 and R 114 R each independently represents a hydrogen atom or a monovalent organic group. 113 and R 114 may contain a polymerizable group, but from the viewpoint of further reducing the dielectric loss tangent, it is preferable that the compound does not contain a radically polymerizable group (particularly a group having an ethylenically unsaturated bond).
[0107] A 1 , A 2 , R 111 , R 113 and R 114 are each independently A in formula (2). 1 , A 2 , R 111 , R 113 and R 114 The same definition and preferred range are also true. 112 is R in formula (5). 112 The same applies to the preferred range.
[0108] The polyimide precursor may contain one type of repeating unit represented by formula (2), or may contain two or more types. It may also contain a structural isomer of the repeating unit represented by formula (2). The polyimide precursor may also contain other types of repeating units in addition to the repeating unit of formula (2).
[0109] In one embodiment of the polyimide precursor of the present invention, the content of the repeating unit represented by formula (2) is 50 mol% or more of all repeating units. The total content is more preferably 70 mol% or more, even more preferably 90 mol% or more, and particularly preferably more than 90 mol%. The upper limit of the total content is not particularly limited, and all repeating units in the polyimide precursor except for the terminal repeating units may be repeating units represented by formula (2).
[0110] The weight-average molecular weight (Mw) of the polyimide precursor is preferably 5,000 to 100,000, more preferably 10,000 to 50,000, and even more preferably 15,000 to 40,000. The number-average molecular weight (Mn) of the polyimide precursor is preferably 2,000 to 40,000, more preferably 3,000 to 30,000, and even more preferably 4,000 to 20,000. The molecular weight dispersity of the polyimide precursor is preferably 1.5 or more, more preferably 1.8 or more, and even more preferably 2.0 or more. The upper limit of the molecular weight dispersity of the polyimide precursor is not particularly specified, but is, for example, preferably 7.0 or less, more preferably 6.5 or less, and even more preferably 6.0 or less. In this specification, the molecular weight dispersity is a value calculated by dividing the weight-average molecular weight by the number-average molecular weight. When the resin composition contains multiple polyimide precursors as specific resins, it is preferable that the weight-average molecular weight, number-average molecular weight, and dispersity of at least one polyimide precursor are within the above-mentioned ranges. It is also preferable that the weight-average molecular weight, number-average molecular weight, and dispersity calculated by treating the multiple polyimide precursors as a single resin are each within the above-mentioned ranges.
[0111] [Polyimide] The polyimide used in the present invention may be an alkali-soluble polyimide, or may be a polyimide soluble in a developer containing an organic solvent as a main component. In this specification, alkali-soluble polyimide refers to a polyimide that dissolves at 0.1 g or more in 100 g of a 2.38 mass % aqueous tetramethylammonium solution at 23°C. From the viewpoint of pattern formability, a polyimide that dissolves at 0.5 g or more is preferred, and a polyimide that dissolves at 1.0 g or more is even more preferred. The upper limit of the solubility is not particularly limited, but is preferably 100 g or less. From the viewpoint of the film strength and insulating properties of the resulting organic film, the polyimide is preferably a polyimide having multiple imide structures in its main chain.
[0112] -Fluorine Atom- From the viewpoint of the film strength of the obtained organic film, it is also preferable that the polyimide contains a fluorine atom. The fluorine atom is, for example, R 132 or R in the repeating unit represented by formula (4) described below 131 and R in the repeating unit represented by formula (4) described below is preferably included. 132 or R in the repeating unit represented by formula (4) described below 131 The amount of fluorine atoms relative to the total mass of the polyimide is preferably 5% by mass or more and 20% by mass or less.
[0113] -Silicon Atom- From the viewpoint of the film strength of the obtained organic film, it is also preferable that the polyimide contains a silicon atom. The silicon atom is, for example, R in the repeating unit represented by formula (4) described later. 131 and R in the repeating unit represented by formula (4) described below is preferably included. 131 It is more preferable that the silicon atom or the organic modified (poly)siloxane structure described below is contained in the polyimide. The silicon atom or the organic modified (poly)siloxane structure may be contained in a side chain of the polyimide, but is preferably contained in the main chain of the polyimide. The amount of silicon atoms relative to the total mass of the polyimide is preferably 1 mass % or more, and more preferably 20 mass % or less.
[0114] - Ethylenically unsaturated bond - From the viewpoint of the film strength of the obtained organic film, it is preferable that the polyimide has an ethylenically unsaturated bond. The polyimide may have the ethylenically unsaturated bond at the end of the main chain or in a side chain, but it is preferable that the ethylenically unsaturated bond is in a side chain. The ethylenically unsaturated bond is preferably radically polymerizable. The ethylenically unsaturated bond is formed by the R 132 or R 131 and R 132 or R 131 Among these, the ethylenically unsaturated bond is more preferably contained as a group having an ethylenically unsaturated bond in R 131 and R 131 Examples of the group having an ethylenically unsaturated bond include a group having an optionally substituted vinyl group directly bonded to an aromatic ring, such as a vinyl group, an allyl group, or a vinylphenyl group, a (meth)acrylamide group, a (meth)acryloyloxy group, and a group represented by the following formula (IV):
[0115]
[0116] In formula (IV), R 20 represents a hydrogen atom, a methyl group, an ethyl group or a methylol group, and is preferably a hydrogen atom or a methyl group.
[0117] In formula (IV), R 21 represents an alkylene group having 2 to 12 carbon atoms, —O—CH 2 CH(OH)CH 2-, -C(=O)O-, -O(C=O)NH-, a (poly)alkyleneoxy group having 2 to 30 carbon atoms (the alkylene group preferably has 2 to 12 carbon atoms, more preferably 2 to 6 carbon atoms, and particularly preferably 2 or 3 carbon atoms; the number of repeating alkyleneoxy groups is preferably 1 to 12, more preferably 1 to 6, and particularly preferably 1 to 3 carbon atoms), or a group combining two or more of these. The alkylene group having 2 to 12 carbon atoms may be any of linear, branched, and cyclic alkylene groups, or alkylene groups represented by a combination thereof. The alkylene group having 2 to 12 carbon atoms is preferably an alkylene group having 2 to 8 carbon atoms, and more preferably an alkylene group having 2 to 4 carbon atoms.
[0118] Among these, R 21 is preferably a group represented by any one of the following formulae (R1) to (R3), and more preferably a group represented by formula (R1).
[0119]
[0120] In formulas (R1) to (R3), L represents a single bond, an alkylene group having 2 to 12 carbon atoms, a (poly)alkyleneoxy group having 2 to 30 carbon atoms, or a group in which two or more of these are bonded together; X represents an oxygen atom or a sulfur atom; * represents a bonding site with another structure; and ● represents R 21 In formulas (R1) to (R3), a preferred embodiment of the alkylene group having 2 to 12 carbon atoms or the (poly)alkyleneoxy group having 2 to 30 carbon atoms as L is R in formula (IV). 21The preferred embodiments are the same as those of the alkylene group having 2 to 12 carbon atoms or the (poly)alkyleneoxy group having 2 to 30 carbon atoms. In formula (R1), X is preferably an oxygen atom. In formulas (R1) to (R3), * has the same meaning as * in formula (IV), and the preferred embodiments are also the same. The structure represented by formula (R1) can be obtained, for example, by reacting a polyimide having a hydroxy group such as a phenolic hydroxy group with a compound having an isocyanato group and an ethylenically unsaturated bond (e.g., 2-isocyanatoethyl methacrylate). The structure represented by formula (R2) can be obtained, for example, by reacting a polyimide having a carboxy group with a compound having a hydroxy group and an ethylenically unsaturated bond (e.g., 2-hydroxyethyl methacrylate). The structure represented by formula (R3) can be obtained, for example, by reacting a polyimide having a hydroxy group such as a phenolic hydroxy group with a compound having a glycidyl group and an ethylenically unsaturated bond (e.g., glycidyl methacrylate).
[0121] In formula (IV), * represents a bonding site to another structure, and is preferably a bonding site to the main chain of the polyimide.
[0122] The amount of ethylenically unsaturated bonds relative to the total mass of the polyimide is preferably 0.0001 to 0.1 mol / g, and more preferably 0.0005 to 0.05 mol / g.
[0123] -Polymerizable group other than a group having an ethylenically unsaturated bond- The polyimide may have a polymerizable group other than a group having an ethylenically unsaturated bond. Examples of the polymerizable group other than a group having an ethylenically unsaturated bond include an epoxy group, a cyclic ether group such as an oxetanyl group, an alkoxymethyl group such as a methoxymethyl group, and a methylol group. Examples of the polymerizable group other than a group having an ethylenically unsaturated bond include R in the repeating unit represented by formula (4) below. 131 The amount of polymerizable groups other than groups having an ethylenically unsaturated bond relative to the total mass of the polyimide is preferably 0.0001 to 0.1 mol / g, and more preferably 0.001 to 0.05 mol / g.
[0124] - Polarity conversion group - The polyimide may have a polarity conversion group such as an acid-decomposable group. The acid-decomposable group in the polyimide is R 113 and R 114 The polarity conversion group is, for example, R in the repeating unit represented by formula (4) described later. 131 , R 132 , contained in the terminals of polyimides, etc.
[0125] -Acid Value- When the polyimide is subjected to alkaline development, from the viewpoint of improving developability, the acid value of the polyimide is preferably 30 mgKOH / g or more, more preferably 50 mgKOH / g or more, and even more preferably 70 mgKOH / g or more. The acid value is preferably 500 mgKOH / g or less, more preferably 400 mgKOH / g or less, and even more preferably 200 mgKOH / g or less. When the polyimide is subjected to development using a developer containing an organic solvent as a main component (e.g., "solvent development"), the acid value of the polyimide is preferably 1 to 35 mgKOH / g, more preferably 2 to 30 mgKOH / g, and even more preferably 5 to 20 mgKOH / g. The acid value is measured by a known method, for example, by the method described in JIS K 0070:1992. From the viewpoint of achieving both storage stability and developability, the acid group contained in the polyimide preferably has a pKa of 0 to 10, more preferably 3 to 8. pKa refers to the equilibrium constant Ka of a dissociation reaction in which a hydrogen ion is released from an acid, expressed as its negative common logarithm, pKa. In this specification, pKa refers to a value calculated using ACD / ChemSketch (registered trademark) unless otherwise specified. For pKa, reference may be made to the value listed in the "Revised 5th Edition Chemistry Handbook: Basics" compiled by the Chemical Society of Japan. When the acid group is a polyvalent acid such as phosphoric acid, the pKa is the first dissociation constant. As such an acid group, the polyimide preferably contains at least one selected from the group consisting of a carboxy group and a phenolic hydroxy group, and more preferably a phenolic hydroxy group.
[0126] -Phenol Hydroxy Group- From the viewpoint of ensuring an appropriate development rate with an alkaline developer, the polyimide preferably has a phenolic hydroxy group. The polyimide may have the phenolic hydroxy group at the end of the main chain or on a side chain. The phenolic hydroxy group can be, for example, R in the repeating unit represented by formula (4) described below. 132 or R 131 The amount of phenolic hydroxy groups relative to the total mass of the polyimide is preferably 0.1 to 30 mol / g, and more preferably 1 to 20 mol / g.
[0127] The polyimide used in the present invention is not particularly limited as long as it is a polymer compound having an imide structure, but it is preferable that it contains a repeating unit represented by the following formula (4).
[0128]
[0129] In formula (4), R 131 represents a divalent organic group, and R 132 represents a tetravalent organic group. When the compound has a polymerizable group, the polymerizable group is 131 and R 132 or may be located at the end of the polyimide as shown in the following formula (4-1) or formula (4-2):
[0130]
[0131] In formula (4-1), R 133 is a polymerizable group, and the other groups have the same meanings as in formula (4).
[0132]
[0133] R 134 and R 135 At least one of the groups is a polymerizable group, and if it is not a polymerizable group, it is an organic group, and the other group has the same meaning as in formula (4).
[0134] Examples of the polymerizable group include the above-mentioned group containing an ethylenically unsaturated bond and a crosslinkable group other than the above-mentioned group having an ethylenically unsaturated bond. 131 represents a divalent organic group. The divalent organic group is R 111 The same examples as those listed above are given, and the preferred ranges are also the same. 131 The diamine residues include those remaining after removal of the amino groups of the diamine. Examples of the diamine include aliphatic, cycloaliphatic, and aromatic diamines. Specific examples include R in the formula (2) of the polyimide precursor. 111 Examples include:
[0135] R 131 is preferably a diamine residue having at least two alkylene glycol units in the main chain, in order to more effectively suppress the occurrence of warping during firing, more preferably a diamine residue containing two or more ethylene glycol chains, propylene glycol chains, or both in one molecule, and even more preferably a diamine residue of the above diamine that does not contain an aromatic ring.
[0136] Examples of diamines containing two or more ethylene glycol chains, propylene glycol chains, or both in one molecule include, but are not limited to, Jeffamine (registered trademark) KH-511, ED-600, ED-900, ED-2003, EDR-148, EDR-176, D-200, D-400, D-2000, and D-4000 (all trade names, manufactured by HUNTSMAN Co., Ltd.), 1-(2-(2-(2-aminopropoxy)ethoxy)propoxy)propan-2-amine, and 1-(1-(1-(2-aminopropoxy)propan-2-yl)oxy)propan-2-amine.
[0137] R 132 represents a tetravalent organic group. The tetravalent organic group is R 115 Examples of the group R are the same as those of the group R, and the preferred ranges are also the same. 115 The four bonds of the tetravalent organic group exemplified by: are bonded to the four —C(═O)— moieties in formula (4) to form a condensed ring.
[0138] R 132 Examples of the tetracarboxylic acid residues include those remaining after removal of the anhydride groups from tetracarboxylic dianhydrides. 115 From the viewpoint of the strength of the organic film, R 132 is preferably an aromatic diamine residue having 1 to 4 aromatic rings.
[0139] R 131 and R 132 It is also preferable that at least one of R 131 Preferred examples of R include 2,2-bis(3-hydroxy-4-aminophenyl)propane, 2,2-bis(3-hydroxy-4-aminophenyl)hexafluoropropane, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, and the above (DA-1) to (DA-18). 132 As the above, (DAA-1) to (DAA-5) are more preferred examples.
[0140] The polyimide preferably contains fluorine atoms in its structure, and the content of fluorine atoms in the polyimide is preferably 10% by mass or more, and more preferably 20% by mass or less.
[0141] To improve adhesion to the substrate, the polyimide may be copolymerized with an aliphatic group having a siloxane structure. Specific examples of the diamine component include bis(3-aminopropyl)tetramethyldisiloxane and bis(p-aminophenyl)octamethylpentasiloxane.
[0142] In order to improve the storage stability of the resin composition, it is preferable that the main chain terminals of the polyimide are blocked with a terminal blocking agent such as a monoamine, an acid anhydride, a monocarboxylic acid, a monoacid chloride compound, or a monoactive ester compound. Among these, it is more preferable to use a monoamine, and preferred monoamine compounds include aniline, 2-ethynylaniline, 3-ethynylaniline, 4-ethynylaniline, 5-amino-8-hydroxyquinoline, 1-hydroxy-7-aminonaphthalene, 1-hydroxy-6-aminonaphthalene, 1-hydroxy-5-aminonaphthalene, 1-hydroxy-4-aminonaphthalene, 2-hydroxy-7-aminonaphthalene, 2-hydroxy-6-aminonaphthalene, 2-hydroxy-5-aminonaphthalene, 1-carboxy-7-aminonaphthalene, 1-carboxy-6-aminonaphthalene, and 1-carboxy 2-5-aminonaphthalene, 2-carboxy-7-aminonaphthalene, 2-carboxy-6-aminonaphthalene, 2-carboxy-5-aminonaphthalene, 2-aminobenzoic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, 4-aminosalicylic acid, 5-aminosalicylic acid, 6-aminosalicylic acid, 2-aminobenzenesulfonic acid, 3-aminobenzenesulfonic acid, 4-aminobenzenesulfonic acid, 3-amino-4,6-dihydroxypyrimidine, 2-aminophenol, 3-aminophenol, 4-aminophenol, 2-aminothiophenol, 3-aminothiophenol, 4-aminothiophenol, etc. Two or more of these may be used, and multiple different terminal groups may be introduced by reacting multiple terminal-capping agents.
[0143] -Imidization rate (ring closure rate)- The imidization rate (also referred to as "ring closure rate") of the polyimide is preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more, from the viewpoint of the film strength, insulating properties, etc. of the resulting organic film. The upper limit of the imidization rate is not particularly limited, and it is sufficient if it is 100% or less. The imidization rate is measured, for example, by the following method. The infrared absorption spectrum of the polyimide is measured, and the absorption peak at 1377 cm due to the imide structure is detected. -1 Next, the peak intensity P1 around 1490 cm-1 The resin was heat-treated at 350 °C for 1 hour, and the infrared absorption spectrum was measured again. -1 The peak intensity P2 around 1490 cm -1 The absorption intensity of the aromatic ring observed near the peak intensity P1 is normalized. Using the normalized values of the obtained peak intensities P1 and P2, the cyclization rate (imidization rate) of the resin can be calculated based on the following formula: Cyclization rate (%) = (normalized value of peak intensity P1 / normalized value of peak intensity P2) × 100
[0144] Polyimide is a polymer in which all repeating units are R 131 and R 132 The repeating unit may contain the repeating unit represented by the above formula (4) in which the combination of R 131 and R 132 The polyimide may contain a repeating unit represented by the formula (4) above, which contains two or more different combinations of repeating units. In addition to the repeating unit represented by the formula (4), the polyimide may contain other types of repeating units. Examples of other types of repeating units include the repeating unit represented by the formula (2) above.
[0145] Polyimides can be synthesized by, for example, reacting a tetracarboxylic dianhydride with a diamine (partially substituted with a monoamine end-capping agent) at low temperature, reacting a tetracarboxylic dianhydride with a diamine (partially substituted with an acid anhydride, monoacid chloride compound, or monoactive ester compound end-capping agent) at low temperature, preparing a diester from a tetracarboxylic dianhydride with an alcohol and then reacting it with a diamine (partially substituted with a monoamine end-capping agent) in the presence of a condensing agent, preparing a diester from a tetracarboxylic dianhydride with an alcohol and then converting the remaining dicarboxylic acid to an acid chloride and reacting it with a diamine (partially substituted with a monoamine end-capping agent), or by completely imidizing the resulting polyimide precursor using a known imidization reaction method, or by terminating the imidization reaction midway to introduce a partial imide structure, or by blending a fully imidized polymer with the polyimide precursor to introduce a partial imide structure. Other known polyimide synthesis methods can also be used.
[0146] The weight-average molecular weight (Mw) of the polyimide is preferably 5,000 to 100,000, more preferably 10,000 to 50,000, and even more preferably 15,000 to 40,000. By setting the weight-average molecular weight to 5,000 or more, the fold resistance of the cured film can be improved. In order to obtain an organic film with excellent mechanical properties (e.g., breaking elongation), the weight-average molecular weight is particularly preferably 15,000 or more. The number-average molecular weight (Mn) of the polyimide is preferably 2,000 to 40,000, more preferably 3,000 to 30,000, and even more preferably 4,000 to 20,000. The molecular weight dispersity of the polyimide is preferably 1.5 or more, more preferably 1.8 or more, and even more preferably 2.0 or more. The upper limit of the molecular weight dispersity of the polyimide is not particularly specified, but is, for example, preferably 7.0 or less, more preferably 6.5 or less, and even more preferably 6.0 or less. When the resin composition contains multiple types of polyimides as specific resins, it is preferable that the weight average molecular weight, number average molecular weight, and dispersity of at least one type of polyimide are within the above ranges. It is also preferable that the weight average molecular weight, number average molecular weight, and dispersity calculated by treating the multiple types of polyimides as one resin are each within the above ranges.
[0147] [Polybenzoxazole Precursor] The polybenzoxazole precursor used in the present invention is not particularly limited with respect to its structure, but preferably contains a repeating unit represented by the following formula (3).
[0148]
[0149] In formula (3), R 121 represents a divalent organic group, and R 122 represents a tetravalent organic group, R 123 and R 124 each independently represents a hydrogen atom or a monovalent organic group.
[0150] In formula (3), R 123 and R 124 are R in formula (2), respectively. 113 In formula (3), R 121represents a divalent organic group. The divalent organic group is preferably a group containing at least one of an aliphatic group and an aromatic group. The aliphatic group is preferably a linear aliphatic group. 121 The dicarboxylic acid residue is preferably a dicarboxylic acid residue. Only one type of dicarboxylic acid residue may be used, or two or more types of dicarboxylic acid residues may be used.
[0151] As the dicarboxylic acid residue, dicarboxylic acids containing an aliphatic group and dicarboxylic acid residues containing an aromatic group are preferred, with dicarboxylic acid residues containing an aromatic group being more preferred. As the dicarboxylic acid containing an aliphatic group, dicarboxylic acids containing a linear or branched (preferably linear) aliphatic group are preferred, with dicarboxylic acids consisting of a linear or branched (preferably linear) aliphatic group and two -COOH groups being more preferred. The number of carbon atoms in the linear or branched (preferably linear) aliphatic group is preferably 2 to 30, more preferably 2 to 25, even more preferably 3 to 20, still more preferably 4 to 15, and particularly preferably 5 to 10. The linear aliphatic group is preferably an alkylene group. Examples of dicarboxylic acids containing a linear aliphatic group include malonic acid, dimethylmalonic acid, ethylmalonic acid, isopropylmalonic acid, di-n-butylmalonic acid, succinic acid, tetrafluorosuccinic acid, methylsuccinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylsuccinic acid, dimethylmethylsuccinic acid, glutaric acid, hexafluoroglutaric acid, 2-methylglutaric acid, 3-methylglutaric acid, 2,2-dimethylglutaric acid, 3,3-dimethylglutaric acid, 3-ethyl-3-methylglutaric acid, adipic acid, octafluoroadipic acid, 3-methyladipic acid, pimelic acid, and 2,2,6,6-tetramethylpimelic acid. , suberic acid, dodecafluorosuberic acid, azelaic acid, sebacic acid, hexadecafluorosebacic acid, 1,9-nonanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, nonadecanedioic acid, eicosanedioctic acid, heneicosanedioctic acid, docosanedioctic acid, tricosanedioctic acid, tetracosanedioctic acid, pentacosanedioctic acid, hexacosanedioctic acid, heptacosanedioctic acid, octacosanedioctic acid, nonacosanedioctic acid, triacontanedioic acid, hentriacontanedioic acid, dotriacontanedioic acid, diglycolic acid, and further dicarboxylic acids represented by the following formula:
[0152]
[0153] (In the formula, Z is a hydrocarbon group having 1 to 6 carbon atoms, and n is an integer of 1 to 6.)
[0154] As the dicarboxylic acid containing an aromatic group, the following dicarboxylic acids having an aromatic group are preferred, and the following dicarboxylic acids consisting of only a group having an aromatic group and two —COOH groups are more preferred.
[0155]
[0156] In the formula, A is —CH 2 -, -O-, -S-, -SO 2 -, -CO-, -NHCO-, -C(CF 3 ) 2 - and -C(CH 3 ) 2 - represents a divalent group selected from the group consisting of, and * each independently represents a bonding site to another structure.
[0157] Specific examples of dicarboxylic acids containing an aromatic group include 4,4'-carbonyldibenzoic acid, 4,4'-dicarboxydiphenyl ether, and terephthalic acid.
[0158] In formula (3), R 122 represents a tetravalent organic group. The tetravalent organic group is R 115 The same definition and preferred range are also true. 122is preferably a group derived from a bisaminophenol derivative, and examples of the group derived from a bisaminophenol derivative include 3,3'-diamino-4,4'-dihydroxybiphenyl, 4,4'-diamino-3,3'-dihydroxybiphenyl, 3,3'-diamino-4,4'-dihydroxydiphenyl sulfone, 4,4'-diamino-3,3'-dihydroxydiphenyl sulfone, bis-(3-amino-4-hydroxyphenyl)methane, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis-(3-amino-4-hydroxyphenyl)hexafluoropropane, 2,2-bis-(4-amino- 3-hydroxyphenyl)hexafluoropropane, bis-(4-amino-3-hydroxyphenyl)methane, 2,2-bis-(4-amino-3-hydroxyphenyl)propane, 4,4'-diamino-3,3'-dihydroxybenzophenone, 3,3'-diamino-4,4'-dihydroxybenzophenone, 4,4'-diamino-3,3'-dihydroxydiphenyl ether, 3,3'-diamino-4,4'-dihydroxydiphenyl ether, 1,4-diamino-2,5-dihydroxybenzene, 1,3-diamino-2,4-dihydroxybenzene, 1,3-diamino-4,6-dihydroxybenzene, etc. These bisaminophenols may be used alone or in combination.
[0159] Among the bisaminophenol derivatives, the following bisaminophenol derivatives having an aromatic group are preferred.
[0160]
[0161] In the formula, X 1 is -O-, -S-, -C(CF 3 ) 2 -, -CH 2 -, -SO 2 R represents a hydrogen atom or a monovalent substituent, preferably a hydrogen atom or a hydrocarbon group, and more preferably a hydrogen atom or an alkyl group. 122 It is also preferable that R is a structure represented by the above formula. 122is a structure represented by the above formula, any two of the four * and # are R 122 are bonding sites with the nitrogen atom to which R is bonded, and the other two are bonding sites with the nitrogen atom to which R is bonded in formula (3). 122 is preferably a bonding site with the oxygen atom to which the two * are bonded, and 122 is a bonding site with the oxygen atom to which the bond is made, and two #s are R 122 is a bonding site with the nitrogen atom to which the bond is made, or two * are R 122 is a bonding site with the nitrogen atom to which the bond is made, and two #s are R 122 is more preferably a bonding site with the oxygen atom to which the two * are bonded, and 122 is a bonding site with the oxygen atom to which the bond is made, and two #s are R 122 is more preferably the bonding site with the nitrogen atom to which is bonded.
[0162] The bisaminophenol derivative is also preferably a compound represented by formula (As).
[0163]
[0164] In formula (A-s), R 1 represents a hydrogen atom, alkylene, substituted alkylene, —O—, —S—, —SO 2 R is -, -CO-, -NHCO-, a single bond, or an organic group selected from the group consisting of the following formula (A-sc): 2 R are either a hydrogen atom, an alkyl group, an alkoxy group, an acyloxy group, or a cyclic alkyl group, and may be the same or different. 3 are either a hydrogen atom, a linear or branched alkyl group, an alkoxy group, an acyloxy group or a cyclic alkyl group, and may be the same or different.
[0165]
[0166] In the organic group selected from the group of formula (A-sc), * indicates that it is bonded to the aromatic ring of the aminophenol group of the bisaminophenol derivative represented by the above formula (As).
[0167] In formula (As), the ortho position of the phenolic hydroxy group, i.e., R 3 It is particularly preferred that the hydroxyl group also has a substituent, as this is thought to bring the carbonyl carbon of the amide bond and the hydroxyl group closer together, further enhancing the effect of achieving a high cyclization rate when cured at low temperatures.
[0168] In formula (A-s), R 2 is an alkyl group, and R 3 is preferably an alkyl group, since this can maintain the effects of high transparency to i-rays and a high cyclization rate when cured at low temperatures.
[0169] In formula (A-s), R 1 It is more preferred that R is alkylene or substituted alkylene. 1 Specific examples of the alkylene and substituted alkylene include linear or branched alkyl groups having 1 to 8 carbon atoms. 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 - is more preferable in that it is possible to obtain a well-balanced polybenzoxazole precursor that has sufficient solubility in solvents while maintaining the effects of high transparency to i-line and a high cyclization rate when cured at low temperature.
[0170] As a method for producing the bisaminophenol derivative represented by Formula (As), reference can be made to, for example, paragraphs
[0085] to
[0094] and Example 1 (paragraphs
[0189] to
[0190] ) of JP2013-256506A, the contents of which are incorporated herein by reference.
[0171] Specific examples of the structure of the bisaminophenol derivative represented by formula (A-s) include those described in paragraphs 0070 to 0080 of JP 2013-256506 A, the contents of which are incorporated herein by reference. Specific examples of the structure of the bisaminophenol derivative represented by formula (A-s) are not limited to these.
[0172] The polybenzoxazole precursor may contain other types of repeating units in addition to the repeating unit of formula (3). The polybenzoxazole precursor preferably contains a diamine residue represented by formula (SL) below as another type of repeating unit, in order to suppress the occurrence of warpage due to ring closure.
[0173]
[0174] In formula (SL), Z has an a-structure and a b-structure, and R 1s is a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, and R 2s is a hydrocarbon group having 1 to 10 carbon atoms, and R 3s , R 4s , R 5s , R 6s At least one of the above is an aromatic group, and the rest are hydrogen atoms or organic groups having 1 to 30 carbon atoms, and they may be the same or different. The polymerization of the a-structure and the b-structure may be block polymerization or random polymerization. The mole percentages of the Z moiety are 5 to 95 mole% for the a-structure, 95 to 5 mole% for the b-structure, and a+b is 100 mole%.
[0175] In formula (SL), preferred Z is R in the b structure. 5s and R 6s is a phenyl group. The molecular weight of the structure represented by formula (SL) is preferably 400 to 4,000, more preferably 500 to 3,000. By setting the molecular weight within the above range, it is possible to more effectively reduce the elastic modulus of the polybenzoxazole precursor after dehydration ring closure, thereby achieving both the effect of suppressing warpage and the effect of improving solvent solubility.
[0176] When the diamine residue represented by formula (SL) is contained as another type of repeating unit, it is also preferable to further contain, as a repeating unit, a tetracarboxylic acid residue remaining after removal of the anhydride group from the tetracarboxylic dianhydride. Examples of such a tetracarboxylic acid residue include R 115 Examples include:
[0177] The weight-average molecular weight (Mw) of the polybenzoxazole precursor is preferably 18,000 to 30,000, more preferably 20,000 to 29,000, and even more preferably 22,000 to 28,000. The number-average molecular weight (Mn) is preferably 7,200 to 14,000, more preferably 8,000 to 12,000, and even more preferably 9,200 to 11,200. The molecular weight dispersity of the polybenzoxazole precursor is preferably 1.4 or more, more preferably 1.5 or more, and even more preferably 1.6 or more. The upper limit of the molecular weight dispersity of the polybenzoxazole precursor is not particularly specified, but is, for example, preferably 2.6 or less, more preferably 2.5 or less, even more preferably 2.4 or less, even more preferably 2.3 or less, and even more preferably 2.2 or less. When the resin composition contains multiple polybenzoxazole precursors as specific resins, it is preferable that the weight-average molecular weight, number-average molecular weight, and dispersity of at least one polybenzoxazole precursor be within the above-mentioned ranges. It is also preferable that the weight-average molecular weight, number-average molecular weight, and dispersity calculated by treating the multiple polybenzoxazole precursors as a single resin be within the above-mentioned ranges.
[0178] [Polybenzoxazole] The polybenzoxazole is not particularly limited as long as it is a polymeric compound having a benzoxazole ring, but is preferably a compound represented by the following formula (X), and more preferably a compound represented by the following formula (X) having a polymerizable group. The polymerizable group is preferably a radically polymerizable group. Alternatively, it may be a compound represented by the following formula (X) having a polarity conversion group such as an acid-decomposable group.
[0179]
[0180] In formula (X), R 133 represents a divalent organic group, and R 134 represents a tetravalent organic group. In the case where a polarity conversion group such as a polymerizable group or an acid-decomposable group is contained, the polarity conversion group such as the polymerizable group or the acid-decomposable group is 133 and R 134or may be located at the end of the polybenzoxazole as shown in the following formula (X-1) or formula (X-2):
[0181]
[0182] In formula (X-1), R 135 and R 136 At least one of the groups is a polarity conversion group such as a polymerizable group or an acid-decomposable group, and if it is not a polarity conversion group such as a polymerizable group or an acid-decomposable group, it is an organic group, and the other group has the same meaning as in formula (X).
[0183]
[0184] In formula (X-2), R 137 is a polarity conversion group such as a polymerizable group or an acid-decomposable group, and the others are substituents, and the other groups have the same meanings as in formula (X).
[0185] The polarity conversion group such as the polymerizable group or the acid-decomposable group is the same as that described above in the description of the polyimide precursor.
[0186] R 133 represents a divalent organic group. Examples of the divalent organic group include an aliphatic group and an aromatic group. Specific examples include R 121 Examples include R 121 is the same as:
[0187] R 134 represents a tetravalent organic group. The tetravalent organic group is R in formula (3) of the polybenzoxazole precursor. 122 Examples include R 122 For example, R 122 The four bonds of the tetravalent organic group exemplified by R 134 is the following organic group, the following structure is formed: In the following structure, * represents the bonding site with the nitrogen atom or oxygen atom in formula (X), respectively.
[0188]
[0189] The oxazolization rate of polybenzoxazole is preferably 85% or more, more preferably 90% or more. The upper limit is not particularly limited, and may be 100%. When the oxazolization rate is 85% or more, film shrinkage due to ring closure that occurs when oxazolized by heating is reduced, and warpage can be more effectively suppressed. The oxazolization rate can be measured, for example, by the following method. The infrared absorption spectrum of polybenzoxazole is measured, and the absorption peak at 1620 cm, which is derived from the oxazole structure, is detected. -1 Next, the peak intensity Q1 around 1490 cm -1 The resin was heat-treated at 350°C for 3 hours, and the infrared absorption spectrum was measured again. -1 The peak intensity Q2 around 1490 cm -1 The peak intensity Q1 is normalized by the absorption intensity of the aromatic ring observed near the peak Q2. Using the normalized values of the peak intensities Q1 and Q2 thus obtained, the cyclization rate (oxazole rate) of the resin can be calculated based on the following formula: Cyclization rate (%) = (normalized value of peak intensity Q1 / normalized value of peak intensity Q2) × 100
[0190] Polybenzoxazole is R 133 and R 134 The repeating units may contain the same combination of the formula (X) above, and R 133 and R 134 The polybenzoxazole may contain repeating units of the formula (X) having two or more different combinations of the repeating units. In addition to the repeating units of the formula (X), the polybenzoxazole may also contain other types of repeating units.
[0191] Polybenzoxazole is, for example, a compound obtained by combining a bisaminophenol derivative and R 133or a compound selected from dicarboxylic acid dichlorides and dicarboxylic acid derivatives of the above dicarboxylic acid to obtain a polybenzoxazole precursor, which is then oxazolized by a known oxazolization reaction method. In the case of a dicarboxylic acid, an activated ester type dicarboxylic acid derivative previously reacted with 1-hydroxy-1,2,3-benzotriazole or the like may be used to increase the reaction yield.
[0192] The weight-average molecular weight (Mw) of the polybenzoxazole is preferably 5,000 to 70,000, more preferably 8,000 to 50,000, and even more preferably 10,000 to 30,000. By increasing the weight-average molecular weight to 5,000 or more, the fold resistance of the cured film can be improved. To obtain an organic film with excellent mechanical properties, the weight-average molecular weight is particularly preferably 20,000 or more. When two or more polybenzoxazoles are contained, it is preferable that the weight-average molecular weight of at least one polybenzoxazole be within the above range. The number-average molecular weight (Mn) of the polybenzoxazole is preferably 7,200 to 14,000, more preferably 8,000 to 12,000, and even more preferably 9,200 to 11,200. The molecular weight dispersity of the polybenzoxazole is preferably 1.4 or more, more preferably 1.5 or more, and even more preferably 1.6 or more. The upper limit of the molecular weight dispersity of polybenzoxazole is not particularly specified, but is, for example, preferably 2.6 or less, more preferably 2.5 or less, even more preferably 2.4 or less, even more preferably 2.3 or less, and even more preferably 2.2 or less. When the resin composition contains multiple types of polybenzoxazole as the specific resin, it is preferable that the weight average molecular weight, number average molecular weight, and dispersity of at least one type of polybenzoxazole are within the above ranges. It is also preferable that the weight average molecular weight, number average molecular weight, and dispersity calculated by treating the multiple types of polybenzoxazole as a single resin are each within the above ranges.
[0193] [Polyamideimide Precursor] The polyamideimide precursor preferably contains a repeating unit represented by the following formula (PAI-2).
[0194]
[0195] In formula (PAI-2), R 117 represents a trivalent organic group, R 111 represents a divalent organic group, A 2 represents an oxygen atom or —NH—, R 113 represents a hydrogen atom or a monovalent organic group.
[0196] In formula (PAI-2), R 117 is exemplified by a linear or branched aliphatic group, a cyclic aliphatic group, an aromatic group, a heteroaromatic group, or a group in which two or more of these are linked by a single bond or a linking group, and is preferably a linear aliphatic group having 2 to 20 carbon atoms, a branched aliphatic group having 3 to 20 carbon atoms, a cyclic aliphatic group having 3 to 20 carbon atoms, an aromatic group having 6 to 20 carbon atoms, or a group in which two or more of these are combined by a single bond or a linking group, and more preferably an aromatic group having 6 to 20 carbon atoms, or a group in which two or more aromatic groups having 6 to 20 carbon atoms are combined by a single bond or a linking group. Examples of the linking group include -O-, -S-, -C(=O)-, -S(=O) 2Preferred are -, an alkylene group, a halogenated alkylene group, an arylene group, or a linking group formed by bonding two or more of these, and more preferred are -O-, -S-, an alkylene group, a halogenated alkylene group, an arylene group, or a linking group formed by bonding two or more of these. The alkylene group is preferably an alkylene group having 1 to 20 carbon atoms, more preferably an alkylene group having 1 to 10 carbon atoms, and even more preferably an alkylene group having 1 to 4 carbon atoms. The halogenated alkylene group is preferably a halogenated alkylene group having 1 to 20 carbon atoms, more preferably a halogenated alkylene group having 1 to 10 carbon atoms, and even more preferably a halogenated alkylene group having 1 to 4 carbon atoms. Furthermore, examples of the halogen atom in the halogenated alkylene group include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, and a fluorine atom is preferred. The halogenated alkylene group may contain hydrogen atoms or may have all of the hydrogen atoms substituted with halogen atoms, but it is preferable that all of the hydrogen atoms be substituted with halogen atoms. Examples of preferred halogenated alkylene groups include a (ditrifluoromethyl)methylene group. The arylene group is preferably a phenylene group or a naphthylene group, more preferably a phenylene group, and even more preferably a 1,3-phenylene group or a 1,4-phenylene group.
[0197] Also, R 117 is preferably derived from a tricarboxylic acid compound in which at least one carboxy group may be halogenated. The halogenation is preferably chlorination. In the present invention, a compound having three carboxy groups is referred to as a tricarboxylic acid compound. Two of the three carboxy groups in the tricarboxylic acid compound may be converted to acid anhydrides. Examples of tricarboxylic acid compounds that may be halogenated and are used in the production of polyamide-imide precursors include branched aliphatic, cyclic aliphatic, and aromatic tricarboxylic acid compounds. These tricarboxylic acid compounds may be used alone or in combination of two or more.
[0198] Specifically, the tricarboxylic acid compound is preferably a tricarboxylic acid compound containing a linear aliphatic group having 2 to 20 carbon atoms, a branched aliphatic group having 3 to 20 carbon atoms, a cyclic aliphatic group having 3 to 20 carbon atoms, an aromatic group having 6 to 20 carbon atoms, or a group in which two or more of these are combined via a single bond or a linking group, and more preferably a tricarboxylic acid compound containing an aromatic group having 6 to 20 carbon atoms, or a group in which two or more aromatic groups having 6 to 20 carbon atoms are combined via a single bond or a linking group.
[0199] Specific examples of tricarboxylic acid compounds include 1,2,3-propanetricarboxylic acid, 1,3,5-pentanetricarboxylic acid, citric acid, trimellitic acid, 2,3,6-naphthalenetricarboxylic acid, and compounds in which phthalic acid (or phthalic anhydride) and benzoic acid are bonded with a single bond, —O—, —CH 2 -, -C(CH 3 ) 2 -, -C(CF 3 ) 2 -, -SO 2 These compounds may be compounds in which two carboxy groups are anhydride (e.g., trimellitic anhydride), or compounds in which at least one carboxy group is halogenated (e.g., trimellitic anhydride chloride).
[0200] In formula (PAI-2), R 111 , A 2 , R 113 are R in the above formula (2), 111 , A 2 , R 113 The same applies to the preferred embodiments.
[0201] The polyamideimide precursor may further contain other repeating units, such as the repeating unit represented by the above formula (2) and the repeating unit represented by the following formula (PAI-1):
[0202]
[0203] In formula (PAI-1), R 116 represents a divalent organic group, R 111represents a divalent organic group. 116 is exemplified by a linear or branched aliphatic group, a cyclic aliphatic group, an aromatic group, a heteroaromatic group, or a group in which two or more of these are linked by a single bond or a linking group, and is preferably a linear aliphatic group having 2 to 20 carbon atoms, a branched aliphatic group having 3 to 20 carbon atoms, a cyclic aliphatic group having 3 to 20 carbon atoms, an aromatic group having 6 to 20 carbon atoms, or a group in which two or more of these are combined by a single bond or a linking group, and more preferably an aromatic group having 6 to 20 carbon atoms, or a group in which two or more aromatic groups having 6 to 20 carbon atoms are combined by a single bond or a linking group. Examples of the linking group include -O-, -S-, -C(=O)-, -S(=O) 2 Preferred are -, an alkylene group, a halogenated alkylene group, an arylene group, or a linking group formed by bonding two or more of these, and more preferred are -O-, -S-, an alkylene group, a halogenated alkylene group, an arylene group, or a linking group formed by bonding two or more of these. The alkylene group is preferably an alkylene group having 1 to 20 carbon atoms, more preferably an alkylene group having 1 to 10 carbon atoms, and even more preferably an alkylene group having 1 to 4 carbon atoms. The halogenated alkylene group is preferably a halogenated alkylene group having 1 to 20 carbon atoms, more preferably a halogenated alkylene group having 1 to 10 carbon atoms, and even more preferably a halogenated alkylene group having 1 to 4 carbon atoms. Furthermore, examples of the halogen atom in the halogenated alkylene group include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, and a fluorine atom is preferred. The halogenated alkylene group may contain hydrogen atoms or may have all of the hydrogen atoms substituted with halogen atoms, but it is preferable that all of the hydrogen atoms be substituted with halogen atoms. Examples of preferred halogenated alkylene groups include a (ditrifluoromethyl)methylene group. The arylene group is preferably a phenylene group or a naphthylene group, more preferably a phenylene group, and even more preferably a 1,3-phenylene group or a 1,4-phenylene group.
[0204] Also, R 116is preferably derived from a dicarboxylic acid compound or a dicarboxylic acid dihalide compound. In the present invention, a compound having two carboxy groups is called a dicarboxylic acid compound, and a compound having two halogenated carboxy groups is called a dicarboxylic acid dihalide compound. The carboxy groups in the dicarboxylic acid dihalide compound may be halogenated, but are preferably chlorinated, for example. That is, the dicarboxylic acid dihalide compound is preferably a dicarboxylic acid dichloride compound. Examples of optionally halogenated dicarboxylic acid compounds or dicarboxylic acid dihalide compounds used in the production of polyamideimide precursors include linear or branched aliphatic, cyclic aliphatic, or aromatic dicarboxylic acid compounds or dicarboxylic acid dihalide compounds. These dicarboxylic acid compounds or dicarboxylic acid dihalide compounds may be used alone or in combination of two or more.
[0205] Specifically, the dicarboxylic acid compound or dicarboxylic acid dihalide compound is preferably a dicarboxylic acid compound or dicarboxylic acid dihalide compound containing a linear aliphatic group having 2 to 20 carbon atoms, a branched aliphatic group having 3 to 20 carbon atoms, a cyclic aliphatic group having 3 to 20 carbon atoms, an aromatic group having 6 to 20 carbon atoms, or a group in which two or more of these are combined via a single bond or a linking group, and more preferably a dicarboxylic acid compound or dicarboxylic acid dihalide compound containing an aromatic group having 6 to 20 carbon atoms, or a group in which two or more aromatic groups having 6 to 20 carbon atoms are combined via a single bond or a linking group.
[0206] Specific examples of dicarboxylic acid compounds include malonic acid, dimethylmalonic acid, ethylmalonic acid, isopropylmalonic acid, di-n-butylmalonic acid, succinic acid, tetrafluorosuccinic acid, methylsuccinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylsuccinic acid, dimethylmethylsuccinic acid, glutaric acid, hexafluoroglutaric acid, 2-methylglutaric acid, 3-methylglutaric acid, 2,2-dimethylglutaric acid, 3,3-dimethylglutaric acid, 3-ethyl-3-methylglutaric acid, adipic acid, octafluoroadipic acid, 3-methyladipic acid, pimelic acid, 2,2,6,6-tetramethylpimelic acid, suberic acid, dodecafluorosuberic acid, azelaic acid, sebacic acid, and hexadecafluoroadipic acid. Examples of the carboxylic acid include fluorosebacic acid, 1,9-nonanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, nonadecanedioic acid, eicosanedicarboxylic acid, heneicosanedicarboxylic acid, docosanedicarboxylic acid, tricosanedicarboxylic acid, tetracosanedicarboxylic acid, pentacosanedicarboxylic acid, hexacosanedicarboxylic acid, heptacosanedicarboxylic acid, octacosanedicarboxylic acid, nonacosanedicarboxylic acid, triacontanedioic acid, hentriacontanedioic acid, dotriacontanedioic acid, diglycolic acid, phthalic acid, isophthalic acid, terephthalic acid, 4,4'-biphenylcarboxylic acid, 4,4'-biphenylcarboxylic acid, 4,4'-dicarboxydiphenyl ether, and benzophenone-4,4'-dicarboxylic acid. Specific examples of the dicarboxylic acid dihalide compound include compounds in which two carboxy groups in the specific examples of the dicarboxylic acid compounds mentioned above are halogenated.
[0207] In formula (PAI-1), R 111 is R in the above formula (2) 111 The same applies to the preferred embodiments.
[0208] The polyamideimide precursor preferably has fluorine atoms in its structure, and the fluorine atom content in the polyamideimide precursor is preferably 10% by mass or more and 20% by mass or less.
[0209] Furthermore, for the purpose of improving adhesion to a substrate, the polyamide-imide precursor may be copolymerized with an aliphatic group having a siloxane structure. Specific examples include those using bis(3-aminopropyl)tetramethyldisiloxane, bis(p-aminophenyl)octamethylpentasiloxane, or the like as a diamine component.
[0210] One embodiment of the polyamideimide precursor of the present invention includes a repeating unit represented by formula (PAI-2), a repeating unit represented by formula (PAI-1), and a repeating unit represented by formula (2). The total content of these repeating units is preferably 50 mol% or more of all repeating units, more preferably 70 mol% or more, even more preferably 90 mol% or more, and particularly preferably more than 90 mol%. The upper limit of the total content is not particularly limited, but is 100 mol% or less. All repeating units in the polyamideimide precursor excluding the terminal repeating units may be any of the repeating units represented by formula (PAI-2), the repeating units represented by formula (PAI-1), and the repeating units represented by formula (2). Another embodiment of the polyamideimide precursor of the present invention includes a repeating unit represented by formula (PAI-2) and a repeating unit represented by formula (PAI-1). The total content of the repeating units is preferably 50 mol% or more, more preferably 70 mol% or more, even more preferably 90 mol% or more, and particularly preferably more than 90 mol% of all repeating units. The upper limit of the total content is not particularly limited, but is 100 mol% or less. All repeating units in the polyamideimide precursor excluding the terminal repeating units may be either repeating units represented by formula (PAI-2) or repeating units represented by formula (PAI-1).
[0211] The weight-average molecular weight (Mw) of the polyamideimide precursor is preferably 2,000 to 500,000, more preferably 5,000 to 100,000, and even more preferably 10,000 to 50,000. The number-average molecular weight (Mn) is preferably 800 to 250,000, more preferably 2,000 to 50,000, and even more preferably 4,000 to 25,000. The molecular weight dispersity of the polyamideimide precursor is preferably 1.5 or more, more preferably 1.8 or more, and even more preferably 2.0 or more. The upper limit of the molecular weight dispersity of the polyamideimide precursor is not particularly specified, but is, for example, preferably 7.0 or less, more preferably 6.5 or less, and even more preferably 6.0 or less. When the resin composition contains multiple types of polyamideimide precursors as the specific resin, it is preferable that the weight-average molecular weight, number-average molecular weight, and dispersity of at least one polyamideimide precursor be within the above-mentioned ranges. It is also preferable that the weight average molecular weight, number average molecular weight, and dispersity, calculated by treating the plurality of types of polyamideimide precursors as one resin, are each within the above-mentioned ranges.
[0212] [Polyamideimide] The polyamideimide used in the present invention may be an alkali-soluble polyamideimide, or may be a polyamideimide soluble in a developer containing an organic solvent as a main component. In this specification, alkali-soluble polyamideimide refers to a polyamideimide that dissolves at 23°C in 100 g of a 2.38% by mass aqueous solution of tetramethylammonium at 0.1 g or more. From the viewpoint of pattern formability, a polyamideimide that dissolves at 0.5 g or more is preferred, and a polyamideimide that dissolves at 1.0 g or more is even more preferred. The upper limit of the solubility is not particularly limited, but is preferably 100 g or less. Furthermore, from the viewpoint of the film strength and insulating properties of the resulting organic film, the polyamideimide is preferably a polyamideimide having multiple amide bonds and multiple imide structures in the main chain.
[0213] -Fluorine Atom- From the viewpoint of the film strength of the obtained organic film, it is preferable that the polyamideimide contains a fluorine atom. The fluorine atom is, for example, R in the repeating unit represented by formula (PAI-3) described later. 117, or R 111 and R in the repeating unit represented by formula (PAI-3) described below is preferably included. 117 , or R 111 The amount of fluorine atoms relative to the total mass of the polyamideimide is preferably 5% by mass or more and 20% by mass or less.
[0214] - Ethylenically unsaturated bond - From the viewpoint of the film strength of the obtained organic film, the polyamideimide may have an ethylenically unsaturated bond. The polyamideimide may have the ethylenically unsaturated bond at the end of the main chain or in a side chain, but it is preferable that the ethylenically unsaturated bond be in a side chain. The ethylenically unsaturated bond is preferably radically polymerizable. The ethylenically unsaturated bond is formed by the R 117 , or R 111 and R in the repeating unit represented by formula (PAI-3) described below is preferably included. 117 , or R 111 It is more preferable that the group having an ethylenically unsaturated bond is contained as a group having an ethylenically unsaturated bond in the following formula: Preferred embodiments of the group having an ethylenically unsaturated bond are the same as the preferred embodiments of the group having an ethylenically unsaturated bond in the polyimide described above.
[0215] The amount of ethylenically unsaturated bonds relative to the total mass of the polyamideimide is preferably 0.0001 to 0.1 mol / g, and more preferably 0.001 to 0.05 mol / g.
[0216] -Polymerizable Group Other Than Ethylenically Unsaturated Bond- The polyamideimide may have a polymerizable group other than an ethylenically unsaturated bond. Examples of the polymerizable group other than an ethylenically unsaturated bond in the polyamideimide include the same groups as the polymerizable group other than an ethylenically unsaturated bond in the polyimide described above. Examples of the polymerizable group other than an ethylenically unsaturated bond include, for example, R 111The amount of polymerizable groups other than ethylenically unsaturated bonds relative to the total mass of the polyamideimide is preferably 0.05 to 10 mol / g, and more preferably 0.1 to 5 mol / g.
[0217] - Polarity conversion group - The polyamideimide may have a polarity conversion group such as an acid-decomposable group. The acid-decomposable group in the polyamideimide is represented by R 113 and R 114 The acid-decomposable group is the same as that described above, and the preferred embodiments are also the same.
[0218] -Acid Value- When the polyamideimide is subjected to alkaline development, from the viewpoint of improving developability, the acid value of the polyamideimide is preferably 30 mgKOH / g or more, more preferably 50 mgKOH / g or more, and even more preferably 70 mgKOH / g or more. Furthermore, the acid value is preferably 500 mgKOH / g or less, more preferably 400 mgKOH / g or less, and even more preferably 200 mgKOH / g or less. Furthermore, when the polyamideimide is subjected to development using a developer containing an organic solvent as a main component (e.g., "solvent development"), the acid value of the polyamideimide is preferably 2 to 35 mgKOH / g, more preferably 3 to 30 mgKOH / g, and even more preferably 5 to 20 mgKOH / g. The acid value is measured by a known method, for example, the method described in JIS K 0070:1992. Furthermore, examples of acid groups contained in the polyamideimide include the same groups as the acid groups in the polyimides described above, and preferred embodiments are also the same.
[0219] -Phenol Hydroxy Group- From the viewpoint of ensuring an appropriate development rate with an alkaline developer, the polyamideimide preferably has a phenolic hydroxy group. The polyamideimide may have the phenolic hydroxy group at the end of the main chain or on a side chain. The phenolic hydroxy group can be, for example, R in the repeating unit represented by formula (PAI-3) described below. 117 , or R 111The amount of phenolic hydroxy groups relative to the total mass of the polyamideimide is preferably 0.1 to 30 mol / g, and more preferably 1 to 20 mol / g.
[0220] The polyamideimide used in the present invention is not particularly limited as long as it is a polymer compound having an imide structure and an amide bond, but it is preferable that it contains a repeating unit represented by the following formula (PAI-3).
[0221]
[0222] In formula (PAI-3), R 111 and R 117 are R in formula (PAI-2), respectively. 111 and R 117 In the case where the polymerizable group is present, the polymerizable group is R 111 and R 117 or may be located at the end of the polyamideimide.
[0223] In order to improve the storage stability of the resin composition, it is preferable to cap the main chain ends of the polyamideimide with a terminal capping agent such as a monoamine, an acid anhydride, a monocarboxylic acid, a monoacid chloride compound, a monoactive ester compound, etc. Preferred embodiments of the terminal capping agent are the same as those of the terminal capping agent for the polyimide described above.
[0224] -Imidization rate (ring closure rate)- The imidization rate (also referred to as "ring closure rate") of polyamideimide is preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more, from the viewpoints of the film strength, insulating properties, etc. of the resulting organic film. The upper limit of the imidization rate is not particularly limited, and it is sufficient if it is 100% or less. The imidization rate is measured by the same method as the ring closure rate of polyimide described above.
[0225] Polyamideimide is R 111 and R 117 The repeating unit may contain the repeating unit represented by the formula (PAI-3) in which the combination of R 111 and R 117The polyamideimide may contain a repeating unit represented by formula (PAI-3) above, which contains two or more different combinations of repeating units. In addition to the repeating unit represented by formula (PAI-3), the polyamideimide may also contain other types of repeating units. Examples of other types of repeating units include the repeating units represented by formula (PAI-1) or formula (PAI-2) above.
[0226] Polyamideimide can be synthesized, for example, by obtaining a polyamideimide precursor by a known method and completely imidizing it using a known imidization reaction method, or by terminating the imidization reaction midway and introducing a partial imide structure, or by blending a completely imidized polymer with the polyamideimide precursor to introduce a partial imide structure.
[0227] The weight-average molecular weight (Mw) of the polyamideimide is preferably 5,000 to 70,000, more preferably 8,000 to 50,000, and even more preferably 10,000 to 30,000. By increasing the weight-average molecular weight to 5,000 or more, the fold resistance of the cured film can be improved. To obtain an organic film with excellent mechanical properties, the weight-average molecular weight is particularly preferably 20,000 or more. The number-average molecular weight (Mn) of the polyamideimide is preferably 800 to 250,000, more preferably 2,000 to 50,000, and even more preferably 4,000 to 25,000. The molecular weight dispersity of the polyamideimide is preferably 1.5 or more, more preferably 1.8 or more, and even more preferably 2.0 or more. There is no particular upper limit for the molecular weight dispersity of the polyamideimide, but for example, it is preferably 7.0 or less, more preferably 6.5 or less, and even more preferably 6.0 or less. When the resin composition contains multiple polyamideimides as specific resins, it is preferable that the weight-average molecular weight, number-average molecular weight, and dispersity of at least one polyamideimide are within the above-mentioned ranges. It is also preferable that the weight-average molecular weight, number-average molecular weight, and dispersity calculated by treating the multiple polyamideimides as a single resin are each within the above-mentioned ranges.
[0228] [Method for Producing Polyimide Precursors, etc.] Polyimide precursors, etc., can be obtained by, for example, reacting a tetracarboxylic dianhydride with a diamine at low temperature, reacting a tetracarboxylic dianhydride with a diamine at low temperature to obtain a polyamic acid and then esterifying the polyamic acid using a condensing agent or an alkylating agent, obtaining a diester from a tetracarboxylic dianhydride with an alcohol and then reacting the diester with a diamine in the presence of a condensing agent, obtaining a diester from a tetracarboxylic dianhydride with an alcohol, then acid-halogenating the remaining dicarboxylic acid with a halogenating agent, and then reacting the diamine with the diamine. Among the above-mentioned production methods, the method of obtaining a diester from a tetracarboxylic dianhydride with an alcohol, then acid-halogenating the remaining dicarboxylic acid with a halogenating agent, and then reacting the diamine with the diamine is more preferred. Examples of the condensing agent include dicyclohexylcarbodiimide, diisopropylcarbodiimide, 1-ethoxycarbonyl-2-ethoxy-1,2-dihydroquinoline, 1,1-carbonyldioxy-di-1,2,3-benzotriazole, N,N'-disuccinimidyl carbonate, and trifluoroacetic anhydride. Examples of the alkylating agent include N,N-dimethylformamide dimethyl acetal, N,N-dimethylformamide diethyl acetal, N,N-dialkylformamide dialkyl acetal, trimethyl orthoformate, and triethyl orthoformate. Examples of the halogenating agent include thionyl chloride, oxalyl chloride, and phosphorus oxychloride. In the method for producing a polyimide precursor or the like, it is preferable to use an organic solvent during the reaction. One or more organic solvents may be used. The organic solvent can be appropriately selected depending on the raw materials, and examples thereof include pyridine, diethylene glycol dimethyl ether (diglyme), N-methylpyrrolidone, N-ethylpyrrolidone, ethyl propionate, dimethylacetamide, dimethylformamide, tetrahydrofuran, and γ-butyrolactone. In the method for producing a polyimide precursor or the like, it is preferable to add a basic compound during the reaction. The basic compound may be one type or two or more types.The basic compound can be appropriately selected depending on the raw material, and examples thereof include triethylamine, diisopropylethylamine, pyridine, 1,8-diazabicyclo[5.4.0]undec-7-ene, and N,N-dimethyl-4-aminopyridine.
[0229] -End-capping agent- In order to further improve storage stability during the production method of a polyimide precursor or the like, it is preferable to cap the carboxylic acid anhydride, acid anhydride derivative, or amino group remaining at the resin terminal of the polyimide precursor or the like. When capping the carboxylic acid anhydride or acid anhydride derivative remaining at the resin terminal, examples of the end-capping agent include monoalcohols, phenols, thiols, thiophenols, monoamines, etc., and in terms of reactivity and film stability, it is more preferable to use monoalcohols, phenols, or monoamines. Preferred monoalcohol compounds include primary alcohols such as methanol, ethanol, propanol, butanol, hexanol, octanol, dodecynol, benzyl alcohol, 2-phenylethanol, 2-methoxyethanol, 2-chloromethanol, and furfuryl alcohol; secondary alcohols such as isopropanol, 2-butanol, cyclohexyl alcohol, cyclopentanol, and 1-methoxy-2-propanol; and tertiary alcohols such as t-butyl alcohol and adamantane alcohol. Preferred phenolic compounds include phenols such as phenol, methoxyphenol, methylphenol, naphthalene-1-ol, naphthalene-2-ol, and hydroxystyrene.Preferred examples of the monoamine compound include aniline, 2-ethynylaniline, 3-ethynylaniline, 4-ethynylaniline, 5-amino-8-hydroxyquinoline, 1-hydroxy-7-aminonaphthalene, 1-hydroxy-6-aminonaphthalene, 1-hydroxy-5-aminonaphthalene, 1-hydroxy-4-aminonaphthalene, 2-hydroxy-7-aminonaphthalene, 2-hydroxy-6-aminonaphthalene, 2-hydroxy-5-aminonaphthalene, 1-carboxy-7-aminonaphthalene, 1-carboxy-6-aminonaphthalene, 1-carboxy-5-aminonaphthalene, Examples of suitable end-capping agents include 2-carboxy-7-aminonaphthalene, 2-carboxy-6-aminonaphthalene, 2-carboxy-5-aminonaphthalene, 2-aminobenzoic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, 4-aminosalicylic acid, 5-aminosalicylic acid, 6-aminosalicylic acid, 2-aminobenzenesulfonic acid, 3-aminobenzenesulfonic acid, 4-aminobenzenesulfonic acid, 3-amino-4,6-dihydroxypyrimidine, 2-aminophenol, 3-aminophenol, 4-aminophenol, 2-aminothiophenol, 3-aminothiophenol, and 4-aminothiophenol. Two or more of these may be used, and multiple end-capping agents may be reacted to introduce multiple different end groups. Furthermore, when capping the amino groups at the resin ends, they can be capped with a compound having a functional group capable of reacting with the amino group. Preferred examples of the capping agent for the amino group include carboxylic acid anhydrides, carboxylic acid chlorides, carboxylic acid bromides, sulfonic acid chlorides, sulfonic acid anhydrides, sulfonic acid carboxylic acid anhydrides, etc., and more preferred are carboxylic acid anhydrides and carboxylic acid chlorides. Preferred carboxylic acid anhydride compounds include acetic anhydride, propionic acid anhydride, oxalic acid anhydride, succinic acid anhydride, maleic acid anhydride, phthalic acid anhydride, benzoic acid anhydride, and 5-norbornene-2,3-dicarboxylic acid anhydride.Preferred examples of carboxylic acid chloride compounds include acetyl chloride, acrylic acid chloride, propionyl chloride, methacrylic acid chloride, pivaloyl chloride, cyclohexanecarbonyl chloride, 2-ethylhexanoyl chloride, cinnamoyl chloride, 1-adamantanecarbonyl chloride, heptafluorobutyryl chloride, stearic acid chloride, and benzoyl chloride.
[0230] -Solid Precipitation- The method for producing a polyimide precursor or the like may include a step of precipitating a solid. Specifically, after filtering out water-absorbing by-products of the dehydration condensation agent coexisting in the reaction solution as needed, the resulting polymer component is poured into a poor solvent such as water, a lower aliphatic alcohol, or a mixture thereof to precipitate the polymer component as a solid, which is then dried to obtain a polyimide precursor or the like. To improve the degree of purification, the polyimide precursor or the like may be repeatedly subjected to operations such as redissolving, reprecipitation, and drying. Furthermore, the method may include a step of removing ionic impurities using an ion exchange resin.
[0231] [Content] The resin content in the resin composition of the present invention is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and even more preferably 50% by mass or more, based on the total solid content of the resin composition. Furthermore, the resin content in the resin composition of the present invention is preferably 99.5% by mass or less, more preferably 99% by mass or less, even more preferably 98% by mass or less, even more preferably 97% by mass or less, and even more preferably 95% by mass or less, based on the total solid content of the resin composition. The resin composition of the present invention may contain only one type of resin, or may contain two or more types. When two or more types are contained, it is preferable that the total amount is within the above range. It is particularly preferable that the resin is a specific resin, and the content of the specific resin is within the above range.
[0232] It is also preferable that the resin composition of the present invention contains at least two kinds of resins. Specifically, the resin composition of the present invention may contain a total of two or more kinds of the specific resin and other resins described later, or may contain two or more kinds of specific resins, but it is preferable that the resin composition of the present invention contains two or more kinds of specific resins. When the resin composition of the present invention contains two or more kinds of specific resins, for example, a polyimide precursor having a structure derived from a dianhydride (R 115 ) preferably contains two or more different polyimide precursors.
[0233] The resin composition of the present invention may contain the above-mentioned specific resin and another resin (hereinafter simply referred to as "other resin") different from the specific resin. Examples of the other resin include phenolic resin, polyamide, epoxy resin, polysiloxane, resin containing a siloxane structure, (meth)acrylic resin, (meth)acrylamide resin, urethane resin, butyral resin, styryl resin, polyether resin, polyester resin, etc. For example, by further adding a (meth)acrylic resin, a resin composition with excellent coatability can be obtained, and a pattern (cured product) with excellent solvent resistance can be obtained. For example, instead of or in addition to the polymerizable compound described below, a polymerizable compound having a high polymerizable group value and a weight average molecular weight of 20,000 or less (for example, a polymerizable group content of 1×10 per 1 g of resin) can be used. -3 By adding a (meth)acrylic resin (having a molecular weight of 1000 to 1000 mol / g or more) to the resin composition, it is possible to improve the coatability of the resin composition and the solvent resistance of the pattern (cured product).
[0234] When the resin composition of the present invention contains another resin, the content of the other resin is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, even more preferably 1% by mass or more, even more preferably 2% by mass or more, even more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on the total solid content of the resin composition. The content of the other resin in the resin composition of the present invention is preferably 80% by mass or less, more preferably 75% by mass or less, even more preferably 70% by mass or less, even more preferably 60% by mass or less, and even more preferably 50% by mass or less, based on the total solid content of the resin composition. A preferred embodiment of the resin composition of the present invention may also be an embodiment in which the content of the other resin is low. In the above embodiment, the content of the other resin is preferably 20% by mass or less, more preferably 15% by mass or less, even more preferably 10% by mass or less, even more preferably 5% by mass or less, and even more preferably 1% by mass or less, based on the total solid content of the resin composition. The lower limit of the content is not particularly limited, as long as it is 0% by mass or more. The resin composition of the present invention may contain only one type of other resin, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0235] <Polymerizable Compound> The resin composition of the present invention may contain a polymerizable compound. Regarding the polymerizable compound, the contents of paragraphs
[0076] to
[0123] of WO 2022 / 210532 are incorporated herein by reference.
[0236] <Polymerization initiator> The resin composition of the present invention may contain a polymerization initiator. With regard to the polymerization initiator, the contents of paragraphs
[0124] to
[0159] of WO 2022 / 210532 are incorporated herein by reference.
[0237] <Sensitizer> The resin composition may contain a sensitizer. The sensitizer absorbs specific actinic radiation and becomes electronically excited. The electronically excited sensitizer comes into contact with a thermal radical polymerization initiator, a photoradical polymerization initiator, or the like, and undergoes actions such as electron transfer, energy transfer, and heat generation. This causes the thermal radical polymerization initiator or the photoradical polymerization initiator to undergo a chemical change and decompose, generating a radical, an acid, or a base. Usable sensitizers include benzophenone-based, Michler's ketone-based, coumarin-based, pyrazole azo-based, anilino azo-based, triphenylmethane-based, anthraquinone-based, anthracene-based, anthrapyridone-based, benzylidene-based, oxonol-based, pyrazolotriazole azo-based, pyridone azo-based, cyanine-based, phenothiazine-based, pyrrolopyrazole azomethine-based, xanthene-based, phthalocyanine-based, benzopyran-based, and indigo-based compounds.Examples of the sensitizer include Michler's ketone, 4,4'-bis(diethylamino)benzophenone, 2,5-bis(4'-diethylaminobenzal)cyclopentane, 2,6-bis(4'-diethylaminobenzal)cyclohexanone, 2,6-bis(4'-diethylaminobenzal)-4-methylcyclohexanone, 4,4'-bis(dimethylamino)chalcone, 4,4'-bis(diethylamino)chalcone, p-dimethylaminocinnamylideneindanone, p-dimethylaminobenzylideneindanone, and Non, 2-(p-dimethylaminophenylbiphenylene)benzothiazole, 2-(p-dimethylaminophenylvinylene)benzothiazole, 2-(p-dimethylaminophenylvinylene)isonaphthothiazole, 1,3-bis(4'-dimethylaminobenzal)acetone, 1,3-bis(4'-diethylaminobenzal)acetone, 3,3'-carbonyl-bis(7-diethylaminocoumarin), 3-acetyl-7-dimethylaminocoumarin, 3-ethoxycarbonyl-7-dimethylaminocoumarin Phosphorus, 3-benzyloxycarbonyl-7-dimethylaminocoumarin, 3-methoxycarbonyl-7-diethylaminocoumarin, 3-ethoxycarbonyl-7-diethylaminocoumarin (ethyl 7-(diethylamino)coumarin-3-carboxylate), N-phenyl-N'-ethylethanolamine, N-phenyldiethanolamine, N-p-tolyldiethanolamine, N-phenylethanolamine, 4-morpholinobenzophenone, isoamyl dimethylaminobenzoate, isoamyl diethylaminobenzoate Examples of sensitizing dyes include soamyl, 2-mercaptobenzimidazole, 1-phenyl-5-mercaptotetrazole, 2-mercaptobenzothiazole, 2-(p-dimethylaminostyryl)benzoxazole, 2-(p-dimethylaminostyryl)benzothiazole, 2-(p-dimethylaminostyryl)naphtho(1,2-d)thiazole, 2-(p-dimethylaminobenzoyl)styrene, diphenylacetamide, benzanilide, N-methylacetanilide, and 3',4'-dimethylacetanilide. Other sensitizing dyes may also be used. For details of sensitizing dyes, please refer to the descriptions in paragraphs 0161 to 0163 of JP-A-2016-027357, the contents of which are incorporated herein by reference.
[0238] When the resin composition contains a sensitizer, the content of the sensitizer is preferably 0.01 to 20 mass %, more preferably 0.1 to 15 mass %, and still more preferably 0.5 to 10 mass %, based on the total solid content of the resin composition. The sensitizer may be used alone or in combination of two or more types.
[0239] <Chain Transfer Agent> The resin composition of the present invention may contain a chain transfer agent. Chain transfer agents are defined, for example, in the Third Edition of the Polymer Dictionary (edited by the Society of Polymer Science, 2005), pages 683-684. Examples of chain transfer agents include those having -S-S-, -SO 2 Compounds having -S-, -N-O-, SH, PH, SiH, and GeH, and dithiobenzoates, trithiocarbonates, dithiocarbamates, xanthate compounds, and the like having a thiocarbonylthio group used in RAFT (Reversible Addition Fragmentation Chain Transfer) polymerization can be used. These compounds can donate hydrogen to a low-activity radical to generate a radical, or can be oxidized and then deprotonated to generate a radical. In particular, thiol compounds can be preferably used.
[0240] In addition, the chain transfer agent may be a compound described in paragraphs 0152 to 0153 of WO 2015 / 199219, the contents of which are incorporated herein by reference.
[0241] When the resin composition contains a chain transfer agent, the content of the chain transfer agent is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the total solid content of the resin composition. Only one type of chain transfer agent may be used, or two or more types may be used. When two or more types of chain transfer agents are used, the total content thereof is preferably within the above range.
[0242] <Base Generator> The resin composition of the present invention may contain a base generator. Here, the base generator is a compound capable of generating a base by physical or chemical action. Preferred base generators include thermal base generators and photobase generators. In particular, when the resin composition contains a precursor of a cyclized resin, the resin composition preferably contains a base generator. By containing a thermal base generator in the resin composition, the cyclization reaction of the precursor can be promoted, for example, by heating, and the mechanical properties and chemical resistance of the cured product can be improved, resulting in excellent performance as an interlayer insulating film for a rewiring layer included in a semiconductor package. The base generator may be an ionic base generator or a nonionic base generator. Examples of the base generated from the base generator include secondary amines and tertiary amines. The base generator is not particularly limited, and known base generators can be used. Examples of known base generators include carbamoyl oxime compounds, carbamoyl hydroxylamine compounds, carbamic acid compounds, formamide compounds, acetamide compounds, carbamate compounds, benzyl carbamate compounds, nitrobenzyl carbamate compounds, sulfonamide compounds, imidazole derivative compounds, amine imide compounds, pyridine derivative compounds, α-aminoacetophenone derivative compounds, quaternary ammonium salt derivative compounds, iminium salts, pyridinium salts, α-lactone ring derivative compounds, amine imide compounds, phthalimide derivative compounds, acyloxyimino compounds, etc. Specific examples of non-ionic base generators include compounds represented by formula (B1), formula (B2), or formula (B3).
[0243]
[0244] In formula (B1) and formula (B2), Rb 1 , Rb 2 and Rb 3 each independently represents an organic group not having a tertiary amine structure, a halogen atom, or a hydrogen atom, provided that Rb 1 and Rb 2 cannot be hydrogen atoms at the same time. 1 , Rb 2 and Rb 3None of the above has a carboxy group. In this specification, the term "tertiary amine structure" refers to a structure in which all three bonds of a trivalent nitrogen atom are covalently bonded to carbon atoms of a hydrocarbon group. Therefore, if the carbon atom bonded to the trivalent nitrogen atom is a carbon atom constituting a carbonyl group, i.e., if it forms an amide group together with the nitrogen atom, it is not a tertiary amine structure.
[0245] In formula (B1) and formula (B2), Rb 1 , Rb 2 and Rb 3 Preferably, at least one of these contains a cyclic structure, and more preferably, at least two contain a cyclic structure. The cyclic structure may be either a monocyclic ring or a fused ring, and a monocyclic ring or a fused ring in which two monocyclic rings are fused is preferred. The monocyclic ring is preferably a 5-membered or 6-membered ring, and more preferably a 6-membered ring. The monocyclic ring is preferably a cyclohexane ring or a benzene ring, and more preferably a cyclohexane ring.
[0246] More specifically, Rb 1 and Rb 2 is preferably a hydrogen atom, an alkyl group (preferably having 1 to 24 carbon atoms, more preferably having 2 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms), an alkenyl group (preferably having 2 to 24 carbon atoms, more preferably having 2 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms), an aryl group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and even more preferably having 6 to 10 carbon atoms), or an arylalkyl group (preferably having 7 to 25 carbon atoms, more preferably having 7 to 19 carbon atoms, and even more preferably having 7 to 12 carbon atoms). These groups may have a substituent. Rb 1 and Rb 2 may be bonded to each other to form a ring. The ring formed is preferably a 4- to 7-membered nitrogen-containing heterocyclic ring. 1 and Rb 2is preferably a linear, branched, or cyclic alkyl group (preferably having 1 to 24 carbon atoms, more preferably having 2 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms) which may have a substituent, more preferably a cycloalkyl group (preferably having 3 to 24 carbon atoms, more preferably having 3 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms) which may have a substituent, and even more preferably a cyclohexyl group which may have a substituent.
[0247] Rb 3 Examples of the alkyl group include an alkyl group (preferably having 1 to 24 carbon atoms, more preferably having 2 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms), an aryl group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and even more preferably having 6 to 10 carbon atoms), an alkenyl group (preferably having 2 to 24 carbon atoms, more preferably having 2 to 12 carbon atoms, and even more preferably having 2 to 6 carbon atoms), an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably having 7 to 19 carbon atoms, and even more preferably having 7 to 12 carbon atoms), an arylalkenyl group (preferably having 8 to 24 carbon atoms, more preferably having 8 to 20 carbon atoms, and even more preferably having 8 to 16 carbon atoms), an alkoxyl group (preferably having 1 to 24 carbon atoms, more preferably having 2 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms), an aryloxy group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and even more preferably having 6 to 12 carbon atoms), and an arylalkyloxy group (preferably having 7 to 23 carbon atoms, more preferably having 7 to 19 carbon atoms, and even more preferably having 7 to 12 carbon atoms). Among these, a cycloalkyl group (preferably having 3 to 24 carbon atoms, more preferably having 3 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms), an arylalkenyl group, and an arylalkyloxy group are preferred. 3 may further have a substituent.
[0248] The compound represented by formula (B1) is preferably a compound represented by the following formula (B1-1) or (B1-2):
[0249]
[0250] In the formula, Rb 11 and Rb 12 , and Rb 31 and Rb 32 respectively represent Rb in formula (B1). 1 and Rb 2 is the same as Rb13 is an alkyl group (preferably having 1 to 24 carbon atoms, more preferably having 2 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms), an alkenyl group (preferably having 2 to 24 carbon atoms, more preferably having 2 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms), an aryl group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and even more preferably having 6 to 12 carbon atoms), or an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably having 7 to 19 carbon atoms, and even more preferably having 7 to 12 carbon atoms), which may have a substituent. 13 is preferably an arylalkyl group.
[0251] Rb 33 and Rb 34 are each independently a hydrogen atom, an alkyl group (preferably having 1 to 12 carbon atoms, more preferably having 1 to 8 carbon atoms, and still more preferably having 1 to 3 carbon atoms), an alkenyl group (preferably having 2 to 12 carbon atoms, more preferably having 2 to 8 carbon atoms, and still more preferably having 2 to 3 carbon atoms), an aryl group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and still more preferably having 6 to 10 carbon atoms), or an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably having 7 to 19 carbon atoms, and still more preferably having 7 to 11 carbon atoms), and a hydrogen atom is preferred.
[0252] Rb 35 represents an alkyl group (preferably having 1 to 24 carbon atoms, more preferably having 1 to 12 carbon atoms, and even more preferably having 3 to 8 carbon atoms), an alkenyl group (preferably having 2 to 12 carbon atoms, more preferably having 2 to 10 carbon atoms, and even more preferably having 3 to 8 carbon atoms), an aryl group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and even more preferably having 6 to 12 carbon atoms), or an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably having 7 to 19 carbon atoms, and even more preferably having 7 to 12 carbon atoms), with an aryl group being preferred.
[0253] The compound represented by formula (B1-1) is preferably a compound represented by formula (B1-1a).
[0254]
[0255] Rb 11 and Rb 12 represents Rb in formula (B1-1). 11 and Rb 12 Rb 15 and Rb16 is a hydrogen atom, an alkyl group (preferably having 1 to 12 carbon atoms, more preferably having 1 to 6 carbon atoms, and even more preferably having 1 to 3 carbon atoms), an alkenyl group (preferably having 2 to 12 carbon atoms, more preferably having 2 to 6 carbon atoms, and even more preferably having 2 to 3 carbon atoms), an aryl group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and even more preferably having 6 to 10 carbon atoms), or an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably having 7 to 19 carbon atoms, and even more preferably having 7 to 11 carbon atoms), and preferably a hydrogen atom or a methyl group. 17 represents an alkyl group (preferably having 1 to 24 carbon atoms, more preferably having 1 to 12 carbon atoms, and even more preferably having 3 to 8 carbon atoms), an alkenyl group (preferably having 2 to 12 carbon atoms, more preferably having 2 to 10 carbon atoms, and even more preferably having 3 to 8 carbon atoms), an aryl group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and even more preferably having 6 to 12 carbon atoms), or an arylalkyl group (preferably having 7 to 23 carbon atoms, more preferably having 7 to 19 carbon atoms, and even more preferably having 7 to 12 carbon atoms), and among these, an aryl group is preferred.
[0256]
[0257] In formula (B3), L represents a divalent hydrocarbon group having a saturated hydrocarbon group on the path of a linking chain connecting adjacent oxygen atoms and carbon atoms, and the number of atoms on the path of the linking chain is 3 or more. N1 and R N2 each independently represents a monovalent organic group.
[0258] In this specification, the term "linking chain" refers to the chain of atoms on the path connecting two atoms or groups of atoms to be linked, which links these atoms or groups of atoms in the shortest possible manner (with the smallest number of atoms). For example, in the compound represented by the following formula, L is composed of a phenyleneethylene group and has an ethylene group as the saturated hydrocarbon group, the linking chain is composed of four carbon atoms, and the number of atoms on the path of the linking chain (i.e., the number of atoms constituting the linking chain, hereinafter also referred to as the "linking chain length" or "length of the linking chain") is 4.
[0259]
[0260] The number of carbon atoms in L in formula (B3) (including carbon atoms other than those in the connecting chain) is preferably 3 to 24. The upper limit is more preferably 12 or less, even more preferably 10 or less, and particularly preferably 8 or less. The lower limit is more preferably 4 or more. From the viewpoint of rapidly progressing the intramolecular cyclization reaction, the upper limit of the connecting chain length of L is preferably 12 or less, more preferably 8 or less, even more preferably 6 or less, and particularly preferably 5 or less. In particular, the connecting chain length of L is preferably 4 or 5, and most preferably 4. Specific preferred compounds for the base generator include, for example, the compounds described in paragraphs 0102 to 0168 of WO 2020 / 066416 and the compounds described in paragraphs 0143 to 0177 of WO 2018 / 038002.
[0261] The base generator also preferably contains a compound represented by the following formula (N1).
[0262]
[0263] In formula (N1), R N1 and R N2 each independently represents a monovalent organic group, R C1 represents a hydrogen atom or a protecting group, and L represents a divalent linking group.
[0264] L is a divalent linking group, and is preferably a divalent organic group. The linking chain length of the linking group is preferably 1 or more, more preferably 2 or more. The upper limit is preferably 12 or less, more preferably 8 or less, and even more preferably 5 or less. The linking chain length is the number of atoms present in the atomic sequence that forms the shortest path between the two carbonyl groups in the formula.
[0265] In formula (N1), R N1 and R N2R each independently represents a monovalent organic group (preferably having 1 to 24 carbon atoms, more preferably having 2 to 18 carbon atoms, and even more preferably having 3 to 12 carbon atoms), and is preferably a hydrocarbon group (preferably having 1 to 24 carbon atoms, more preferably having 1 to 12 carbon atoms, and even more preferably having 1 to 10 carbon atoms). Specific examples include an aliphatic hydrocarbon group (preferably having 1 to 24 carbon atoms, more preferably having 1 to 12 carbon atoms, and even more preferably having 1 to 10 carbon atoms) or an aromatic hydrocarbon group (preferably having 6 to 22 carbon atoms, more preferably having 6 to 18 carbon atoms, and even more preferably having 6 to 10 carbon atoms), and an aliphatic hydrocarbon group is preferred. N1 and R N2 When an aliphatic hydrocarbon group is used as the base, the basicity of the generated base is high, and this is preferable. The aliphatic hydrocarbon group and the aromatic hydrocarbon group may have a substituent, and the aliphatic hydrocarbon group and the aromatic hydrocarbon group may have an oxygen atom in the aliphatic hydrocarbon chain, in the aromatic ring, or in the substituent. In particular, an embodiment in which the aliphatic hydrocarbon group has an oxygen atom in the hydrocarbon chain is exemplified.
[0266] R N1 and R N2Examples of the aliphatic hydrocarbon group constituting the alkyl group include linear or branched chain alkyl groups, cyclic alkyl groups, groups containing a combination of a linear alkyl group and a cyclic alkyl group, and alkyl groups having an oxygen atom in the chain. The linear or branched chain alkyl group preferably has 1 to 24 carbon atoms, more preferably 2 to 18 carbon atoms, and even more preferably 3 to 12 carbon atoms. Examples of the linear or branched chain alkyl group include methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, isopropyl, isobutyl, secondary butyl, tertiary butyl, isopentyl, neopentyl, tertiary pentyl, and isohexyl groups. The cyclic alkyl group preferably has 3 to 12 carbon atoms, more preferably 3 to 6 carbon atoms. Examples of the cyclic alkyl group include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, and cyclooctyl groups. The group containing a combination of a chain alkyl group and a cyclic alkyl group preferably has 4 to 24 carbon atoms, more preferably 4 to 18 carbon atoms, and even more preferably 4 to 12 carbon atoms. Examples of the group containing a combination of a chain alkyl group and a cyclic alkyl group include a cyclohexylmethyl group, a cyclohexylethyl group, a cyclohexylpropyl group, a methylcyclohexylmethyl group, and an ethylcyclohexylethyl group. The alkyl group having an oxygen atom in the chain preferably has 2 to 12 carbon atoms, more preferably 2 to 6 carbon atoms, and even more preferably 2 to 4 carbon atoms. The alkyl group having an oxygen atom in the chain may be chain or cyclic, and may be linear or branched. In particular, from the viewpoint of increasing the boiling point of the decomposition product base described below, R N1 and R N2 is preferably an alkyl group having 5 to 12 carbon atoms. However, in a formulation where importance is placed on adhesion when laminating with a metal (e.g., copper) layer, a group having a cyclic alkyl group or an alkyl group having 1 to 8 carbon atoms is preferred.
[0267] R N1 and R N2 may be linked to each other to form a cyclic structure. The cyclic structure may have an oxygen atom or the like in the chain. N1 and R N2The cyclic structure formed by may be a monocyclic ring or a fused ring, but is preferably a monocyclic ring. The cyclic structure formed is preferably a 5- or 6-membered ring containing a nitrogen atom in formula (N1), for example, a pyrrole ring, an imidazole ring, a pyrazole ring, a pyrroline ring, a pyrrolidine ring, an imidazolidine ring, a pyrazolidine ring, a piperidine ring, a piperazine ring, a morpholine ring, etc., and preferred examples include a pyrroline ring, a pyrrolidine ring, a piperidine ring, a piperazine ring, and a morpholine ring.
[0268] R C1 represents a hydrogen atom or a protecting group, preferably a hydrogen atom. The protecting group is preferably a protecting group that decomposes under the action of an acid or a base, and preferably a protecting group that decomposes with an acid. Specific examples of the protecting group include linear or cyclic alkyl groups and linear or cyclic alkyl groups having an oxygen atom in the chain. Examples of linear or cyclic alkyl groups include a methyl group, an ethyl group, an isopropyl group, a tert-butyl group, and a cyclohexyl group. Examples of linear alkyl groups having an oxygen atom in the chain include alkyloxyalkyl groups, and preferred are a methyloxymethyl (MOM) group and an ethyloxyethyl (EE) group. Examples of cyclic alkyl groups having an oxygen atom in the chain include an epoxy group, a glycidyl group, an oxetanyl group, a tetrahydrofuranyl group, and a tetrahydropyranyl (THP) group.
[0269] In formula (N1), the divalent linking group constituting L is not particularly limited, but is preferably a hydrocarbon group, and more preferably an aliphatic hydrocarbon group. The hydrocarbon group may have a substituent and may have atoms other than carbon atoms in the hydrocarbon chain. The divalent linking group is more preferably a divalent hydrocarbon linking group that may have an oxygen atom in the chain, more preferably a divalent aliphatic hydrocarbon group that may have an oxygen atom in the chain, a divalent aromatic hydrocarbon group, or a group containing a combination of a divalent aliphatic hydrocarbon group that may have an oxygen atom in the chain and a divalent aromatic hydrocarbon group, and even more preferably a divalent aliphatic hydrocarbon group that may have an oxygen atom in the chain. These groups may not have an oxygen atom. The divalent hydrocarbon linking group preferably has 1 to 24 carbon atoms, more preferably 2 to 12 carbon atoms, and even more preferably 2 to 6 carbon atoms. The divalent aliphatic hydrocarbon group preferably has 1 to 12 carbon atoms, more preferably 2 to 6 carbon atoms, and even more preferably 2 to 4 carbon atoms. The divalent aromatic hydrocarbon group preferably has 6 to 22 carbon atoms, more preferably 6 to 18, and even more preferably 6 to 10. The group containing a combination of a divalent aliphatic hydrocarbon group and a divalent aromatic hydrocarbon group (for example, an arylene alkyl group) preferably has 7 to 22 carbon atoms, more preferably 7 to 18, and even more preferably 7 to 10 carbon atoms.
[0270] Specific examples of the linking group L include linear or branched chain alkylene groups, cyclic alkylene groups, groups containing a combination of linear alkylene groups and cyclic alkylene groups, alkylene groups having an oxygen atom in the chain, linear or branched chain alkenylene groups, cyclic alkenylene groups, arylene groups, and arylene alkylene groups. The linear or branched chain alkylene groups preferably have 1 to 12 carbon atoms, more preferably 2 to 6, and even more preferably 2 to 4. The cyclic alkylene groups preferably have 3 to 12 carbon atoms, more preferably 3 to 6. The groups containing a combination of linear alkylene groups and cyclic alkylene groups preferably have 4 to 24 carbon atoms, more preferably 4 to 12, and even more preferably 4 to 6. The alkylene groups having an oxygen atom in the chain may be linear or cyclic, linear or branched. The alkylene group having an oxygen atom in the chain preferably has 1 to 12 carbon atoms, more preferably 1 to 6 carbon atoms, and even more preferably 1 to 3 carbon atoms.
[0271] The linear or branched chain alkenylene group preferably has 2 to 12 carbon atoms, more preferably 2 to 6, and even more preferably 2 to 3. The linear or branched chain alkenylene group preferably has 1 to 10 C═C bonds, more preferably 1 to 6, and even more preferably 1 to 3. The cyclic alkenylene group preferably has 3 to 12 carbon atoms, more preferably 3 to 6. The cyclic alkenylene group preferably has 1 to 6 C═C bonds, more preferably 1 to 4, and even more preferably 1 to 2. The arylene group preferably has 6 to 22 carbon atoms, more preferably 6 to 18, and even more preferably 6 to 10. The arylene alkylene group preferably has 7 to 23 carbon atoms, more preferably 7 to 19, and even more preferably 7 to 11. Among these, a chain alkylene group, a cyclic alkylene group, an alkylene group having an oxygen atom in the chain, a chain alkenylene group, an arylene group, and an arylene alkylene group are preferred, and a 1,2-ethylene group, a propanediyl group (particularly a 1,3-propanediyl group), a cyclohexanediyl group (particularly a 1,2-cyclohexanediyl group), a vinylene group (particularly a cis-vinylene group), a phenylene group (1,2-phenylene group), a phenylenemethylene group (particularly a 1,2-phenylenemethylene group), and an ethyleneoxyethylene group (particularly a 1,2-ethyleneoxy-1,2-ethylene group) are more preferred.
[0272] Examples of the base generator include, but are not limited to, the following compounds:
[0273]
[0274] The molecular weight of the nonionic base generator is preferably 800 or less, more preferably 600 or less, and even more preferably 500 or less. The lower limit is preferably 100 or more, more preferably 200 or more, and even more preferably 300 or more.
[0275] Specific preferred compounds for the ionic base generator include, for example, the compounds described in paragraphs 0148 to 0163 of WO 2018 / 038002.
[0276] Specific examples of ammonium salts include, but are not limited to, the following compounds:
[0277]
[0278] Specific examples of iminium salts include, but are not limited to, the following compounds:
[0279]
[0280] When the resin composition contains a base generator, the content of the base generator is preferably 0.1 to 50 parts by mass per 100 parts by mass of the resin in the resin composition. The lower limit is more preferably 0.3 parts by mass or more, and even more preferably 0.5 parts by mass or more. The upper limit is more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, even more preferably 10 parts by mass or less, even more preferably 5 parts by mass or less, and particularly preferably 4 parts by mass or less. One or more types of base generators can be used. When two or more types are used, the total amount is preferably within the above range.
[0281] <Solvent> The resin composition of the present invention preferably contains a solvent. Any known solvent can be used as the solvent. The solvent is preferably an organic solvent. Examples of the organic solvent include compounds such as esters, ethers, ketones, cyclic hydrocarbons, sulfoxides, amides, ureas, and alcohols.
[0282] Examples of esters include ethyl acetate, n-butyl acetate, isobutyl acetate, hexyl acetate, amyl formate, isoamyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate, ethyl lactate, γ-butyrolactone, ε-caprolactone, δ-valerolactone, alkyl alkyloxyacetates (for example, methyl alkyloxyacetate, ethyl alkyloxyacetate, butyl alkyloxyacetate (for example, methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate, ethyl ethoxyacetate, etc.)), alkyl 3-alkyloxypropionates (for example, methyl 3-alkyloxypropionate, ethyl 3-alkyloxypropionate (for example, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, etc.)), 2-alkyloxypropionates, Preferred examples of the alkyl cypropionate include alkyl cypropionates (e.g., methyl 2-alkyloxypropionate, ethyl 2-alkyloxypropionate, and propyl 2-alkyloxypropionate (e.g., methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, methyl 2-ethoxypropionate, and ethyl 2-ethoxypropionate)), methyl 2-alkyloxy-2-methylpropionate and ethyl 2-alkyloxy-2-methylpropionate (e.g., methyl 2-methoxy-2-methylpropionate and ethyl 2-ethoxy-2-methylpropionate), methyl pyruvate, ethyl pyruvate, propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, methyl 2-oxobutanoate, ethyl 2-oxobutanoate, ethyl hexanoate, ethyl heptanoate, dimethyl malonate, and diethyl malonate.
[0283] Suitable examples of ethers include ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol ethyl methyl ether, diethylene glycol butyl methyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol dimethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether, ethylene glycol monobutyl ether acetate, diethylene glycol ethyl methyl ether, propylene glycol monopropyl ether acetate, and dipropylene glycol dimethyl ether.
[0284] Suitable examples of ketones include methyl ethyl ketone, cyclohexanone, cyclopentanone, 2-heptanone, 3-heptanone, 3-methylcyclohexanone, levoglucosenone, and dihydrolevoglucosenone.
[0285] Suitable examples of cyclic hydrocarbons include aromatic hydrocarbons such as toluene, xylene, and anisole, and cyclic terpenes such as limonene.
[0286] A preferred example of the sulfoxides is dimethyl sulfoxide.
[0287] Preferred examples of the amides include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, N,N-dimethylisobutyramide, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, N-formylmorpholine, and N-acetylmorpholine.
[0288] Preferred examples of ureas include N,N,N',N'-tetramethylurea and 1,3-dimethyl-2-imidazolidinone.
[0289] Examples of alcohols include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 1-pentanol, 1-hexanol, benzyl alcohol, ethylene glycol monomethyl ether, 1-methoxy-2-propanol, 2-ethoxyethanol, diethylene glycol monoethyl ether, diethylene glycol monohexyl ether, triethylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether, polyethylene glycol monomethyl ether, polypropylene glycol, tetraethylene glycol, ethylene glycol monobutyl ether, ethylene glycol monobenzyl ether, ethylene glycol monophenyl ether, methylphenyl carbinol, n-amyl alcohol, methyl amyl alcohol, and diacetone alcohol.
[0290] From the viewpoint of improving the properties of the coated surface, it is also preferable to mix two or more kinds of solvents.
[0291] In the present invention, one solvent selected from methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl cellosolve acetate, ethyl lactate, diethylene glycol dimethyl ether, butyl acetate, methyl 3-methoxypropionate, 2-heptanone, cyclohexanone, cyclopentanone, γ-butyrolactone, γ-valerolactone, 3-methoxy-N,N-dimethylpropionamide, toluene, dimethyl sulfoxide, ethyl carbitol acetate, butyl carbitol acetate, N-methyl-2-pyrrolidone, propylene glycol methyl ether, propylene glycol methyl ether acetate, levoglucosenone, and dihydrolevoglucosenone, or a mixed solvent composed of two or more solvents, is preferred. Particularly preferred are a combination of dimethyl sulfoxide and γ-butyrolactone, a combination of dimethyl sulfoxide and γ-valerolactone, a combination of 3-methoxy-N,N-dimethylpropionamide and γ-butyrolactone, a combination of 3-methoxy-N,N-dimethylpropionamide, γ-butyrolactone and dimethyl sulfoxide, or a combination of N-methyl-2-pyrrolidone and ethyl lactate. An embodiment in which toluene is further added to these combined solvents in an amount of approximately 1 to 10% by mass, based on the total mass of the solvent, is also a preferred embodiment of the present invention. In particular, from the viewpoint of the storage stability of the resin composition, an embodiment in which γ-valerolactone is included as a solvent is also a preferred embodiment of the present invention. In such an embodiment, the content of γ-valerolactone relative to the total mass of the solvent is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. The upper limit of the above content is not particularly limited and may be 100% by mass. The above content may be determined taking into consideration the solubility of components such as the specific resin contained in the resin composition, etc. Furthermore, when dimethyl sulfoxide and γ-valerolactone are used in combination, the solvent preferably contains 60 to 90 mass% of γ-valerolactone and 10 to 40 mass% of dimethyl sulfoxide, more preferably 70 to 90 mass% of γ-valerolactone and 10 to 30 mass% of dimethyl sulfoxide, and even more preferably 75 to 85 mass% of γ-valerolactone and 15 to 25 mass% of dimethyl sulfoxide, relative to the total mass of the solvent.
[0292] From the viewpoint of coatability, the content of the solvent is preferably an amount such that the total solids concentration of the resin composition of the present invention is 5 to 80 mass%, more preferably an amount such that the total solids concentration is 5 to 75 mass%, even more preferably an amount such that the total solids concentration is 10 to 70 mass%, and even more preferably an amount such that the total solids concentration is 20 to 70 mass%. The solvent content may be adjusted depending on the desired thickness of the coating film and the coating method. When two or more solvents are contained, the total amount of the solvents is preferably within the above range.
[0293] <Metal Adhesion Improver> The resin composition of the present invention preferably contains a metal adhesion improver from the viewpoint of improving adhesion to metal materials used in electrodes, wiring, etc. Examples of the metal adhesion improver include a silane coupling agent having an alkoxysilyl group, an aluminum-based adhesion aid, a titanium-based adhesion aid, a compound having a sulfonamide structure, a compound having a thiourea structure, a phosphoric acid derivative compound, a β-ketoester compound, and an amino compound.
[0294] [Silane Coupling Agent] Examples of silane coupling agents include the compounds described in paragraph 0316 of WO 2021 / 112189 and the compounds described in paragraphs 0067 to 0078 of JP 2018-173573, the contents of which are incorporated herein by reference. It is also preferable to use two or more different silane coupling agents, as described in paragraphs 0050 to 0058 of JP 2011-128358 A. It is also preferable to use the following compound as the silane coupling agent. In the following formula, Me represents a methyl group, and Et represents an ethyl group.
[0295]
[0296] Other silane coupling agents include, for example, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, N-2- (aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, tris-(trimethoxysilylpropyl)isocyanurate, 3-ureidopropyltrialkoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, and 3-trimethoxysilylpropylsuccinic anhydride. These can be used alone or in combination of two or more.
[0297] [Aluminum-Based Adhesion Aid] Examples of aluminum-based adhesion aids include aluminum tris(ethylacetoacetate), aluminum tris(acetylacetonate), and ethylacetoacetate aluminum diisopropylate.
[0298] Other metal adhesion improvers that can be used include the compounds described in paragraphs 0046 to 0049 of JP-A-2014-186186 and the sulfide-based compounds described in paragraphs 0032 to 0043 of JP-A-2013-072935, the contents of which are incorporated herein by reference.
[0299] The content of the metal adhesion improver is preferably 0.01 to 30 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the resin. By ensuring that the content is equal to or greater than the above lower limit, the adhesion between the pattern and the metal layer is improved, and by ensuring that the content is equal to or less than the above upper limit, the heat resistance and mechanical properties of the pattern are improved. Only one type of metal adhesion improver may be used, or two or more types may be used. When two or more types are used, it is preferable that the total amount is within the above range.
[0300] <Polymerization Inhibitor> The resin composition of the present invention may contain a polymerization inhibitor. Examples of the polymerization inhibitor include phenolic compounds, quinone compounds, amino compounds, N-oxyl free radical compounds, nitro compounds, nitroso compounds, heteroaromatic ring compounds, and metal compounds.
[0301] Specific examples of the polymerization inhibitor include the compounds described in paragraph 0310 of WO 2021 / 112189, p-hydroquinone, o-hydroquinone, 4-hydroxy-2,2,6,6-tetramethylpiperidine 1-oxyl free radical, and phenoxazine, the contents of which are incorporated herein by reference.
[0302] When the resin composition of the present invention contains a polymerization inhibitor, the content of the polymerization inhibitor is preferably 0.01 to 20 mass%, more preferably 0.02 to 15 mass%, and even more preferably 0.05 to 10 mass%, based on the total solid content of the resin composition.
[0303] The polymerization inhibitor may be one kind or two or more kinds. When two or more kinds of polymerization inhibitors are used, the total amount thereof is preferably within the above range.
[0304] <Acid Scavenger> The resin composition of the present invention preferably contains an acid scavenger to reduce performance changes over time from exposure to heating. Here, the acid scavenger refers to a compound capable of capturing generated acid by its presence in the system, and is preferably a compound with low acidity and high pKa. The acid scavenger is preferably a compound having an amino group, and is preferably a primary amine, a secondary amine, a tertiary amine, an ammonium salt, or a tertiary amide. Primary amines, secondary amines, tertiary amines, or ammonium salts are preferred, with secondary amines, tertiary amines, or ammonium salts being more preferred. Preferred examples of the acid scavenger include compounds having an imidazole structure, a diazabicyclo structure, an onium structure, a trialkylamine structure, an aniline structure, or a pyridine structure, alkylamine derivatives having a hydroxyl group and / or an ether bond, and aniline derivatives having a hydroxyl group and / or an ether bond. When the acid scavenger has an onium structure, it is preferably a salt having a cation selected from ammonium, diazonium, iodonium, sulfonium, phosphonium, pyridinium, or the like, and an anion of an acid less acidic than the acid generated by the acid generator.
[0305] Examples of acid scavengers having an imidazole structure include imidazole, 2,4,5-triphenylimidazole, benzimidazole, and 2-phenylbenzimidazole. Examples of acid scavengers having a diazabicyclo structure include 1,4-diazabicyclo[2,2,2]octane, 1,5-diazabicyclo[4,3,0]non-5-ene, and 1,8-diazabicyclo[5,4,0]undec-7-ene. Examples of acid scavengers having an onium structure include tetrabutylammonium hydroxide, triarylsulfonium hydroxide, phenacylsulfonium hydroxide, and sulfonium hydroxides having a 2-oxoalkyl group, specifically triphenylsulfonium hydroxide, tris(t-butylphenyl)sulfonium hydroxide, bis(t-butylphenyl)iodonium hydroxide, phenacylthiophenium hydroxide, and 2-oxopropylthiophenium hydroxide. Examples of acid scavengers having a trialkylamine structure include tri(n-butyl)amine and tri(n-octyl)amine. Examples of acid scavengers having an aniline structure include 2,6-diisopropylaniline, N,N-dimethylaniline, N,N-dibutylaniline, and N,N-dihexylaniline. Examples of acid scavengers having a pyridine structure include pyridine and 4-methylpyridine. Examples of alkylamine derivatives having a hydroxyl group and / or an ether bond include ethanolamine, diethanolamine, triethanolamine, N-phenyldiethanolamine, and tris(methoxyethoxyethyl)amine. Examples of aniline derivatives having a hydroxyl group and / or an ether bond include N,N-bis(hydroxyethyl)aniline.
[0306] Specific examples of preferred acid scavengers include ethanolamine, diethanolamine, triethanolamine, ethylamine, diethylamine, triethylamine, hexylamine, dodecylamine, cyclohexylamine, cyclohexylmethylamine, cyclohexyldimethylamine, aniline, N-methylaniline, N,N-dimethylaniline, diphenylamine, pyridine, butylamine, isobutylamine, dibutylamine, tributylamine, dicyclohexylamine, DBU (diazabicycloundecene), DABCO (1,4-diazabicyclo[2.2.2]octane), N,N-diisopropylethylamine, tetramethylammonium hydroxide, ethylenediamine, 1,5-diaminopentane ... diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, diphenylamine, ethylhexylamine, N-methyldicyclohexylamine, trioctylamine, N-ethylethylenediamine, N,N-diethylethylenediamine, N,N,N',N'-tetrabutyl-1,6-hexanediamine, spermidine, diaminocyclohexane, bis(2-methoxyethyl)amine, piperidine, methylpiperidine, piperazine, tropane, N-phenylbenzylamine, 1,2-dianilinoethane, 2-aminoethanol, toluidine, aminophenol, hexylaniline, phenylenediamine, phenylethylamine, dibenzylamine, pyrrole, N-methylpyrrole, guanidine, aminopyrrolidine, pyrazole, pyrazoline, aminomorpholine, aminoalkylmorpholine, and the like.
[0307] The resin composition of the present invention may contain an acid scavenger, but if it does contain an acid scavenger, the content of the acid scavenger is preferably 0.001 to 10 mass %, more preferably 0.01 to 5 mass %, based on the total solid content of the resin composition.
[0308] The ratio of the acid generator to the acid scavenger used is preferably acid generator / acid scavenger (molar ratio) = 2.5 to 300. That is, from the viewpoints of sensitivity and resolution, the molar ratio is preferably 2.5 or more, and from the viewpoint of suppressing a decrease in resolution due to thickening of the relief pattern over time after exposure until heat treatment, it is preferably 300 or less. The acid generator / acid scavenger (molar ratio) is preferably 5.0 to 200, more preferably 7.0 to 150.
[0309] <Other Additives> The resin composition of the present invention may contain various additives, such as surfactants, higher fatty acid derivatives, thermal polymerization initiators, inorganic particles, UV absorbers, organic titanium compounds, antioxidants, anti-aggregation agents, phenolic compounds, other polymeric compounds, plasticizers, and other auxiliary agents (e.g., antifoaming agents, flame retardants, etc.), as needed, within the scope of obtaining the effects of the present invention. By appropriately incorporating these components, properties such as film physical properties can be adjusted. For details of these components, please refer to, for example, paragraphs 0183 and after of JP 2012-003225 A (corresponding to paragraph 0237 of U.S. Patent Application Publication No. 2013 / 0034812), and paragraphs 0101 to 0104, 0107 to 0109, etc. of JP 2008-250074 A, the contents of which are incorporated herein by reference. When these additives are incorporated, the total content is preferably 3% by mass or less of the solid content of the resin composition of the present invention.
[0310] [Surfactant] Various surfactants can be used as the surfactant, such as a fluorine-based surfactant, a silicone-based surfactant, a hydrocarbon-based surfactant, etc. The surfactant may be a nonionic surfactant, a cationic surfactant, or an anionic surfactant.
[0311] By including a surfactant in the photosensitive resin composition of the present invention, the liquid properties (particularly fluidity) of the coating liquid composition when prepared can be further improved, and the uniformity of the coating thickness and the liquid saving can be further improved. That is, when a film is formed using a coating liquid containing a surfactant, the interfacial tension between the surface to be coated and the coating liquid is reduced, improving the wettability of the surface to be coated and the coatability of the surface to be coated. Therefore, it is possible to more suitably form a uniform film with little thickness unevenness.
[0312] Examples of fluorine-based surfactants include the compounds described in paragraph 0328 of WO 2021 / 112189, the contents of which are incorporated herein by reference. As the fluorine-based surfactant, fluorine-containing polymer compounds containing a repeating unit derived from a (meth)acrylate compound having a fluorine atom and a repeating unit derived from a (meth)acrylate compound having two or more (preferably five or more) alkyleneoxy groups (preferably ethyleneoxy groups, propyleneoxy groups) can also be preferably used, and examples thereof include the following compounds.
[0313]
[0314] The weight-average molecular weight of the above compound is preferably 3,000 to 50,000, and more preferably 5,000 to 30,000. As the fluorosurfactant, a fluorine-containing polymer having an ethylenically unsaturated group in the side chain can also be used. Specific examples include the compounds described in paragraphs 0050 to 0090 and 0289 to 0295 of JP 2010-164965 A, the contents of which are incorporated herein by reference. Commercially available products include Megafac RS-101, RS-102, and RS-718K manufactured by DIC Corporation.
[0315] The fluorine content in the fluorine-containing surfactant is preferably 3 to 40% by mass, more preferably 5 to 30% by mass, and particularly preferably 7 to 25% by mass. A fluorine-containing surfactant having a fluorine content within this range is effective in terms of uniformity of the thickness of the coating film and liquid saving, and also has good solubility in the composition.
[0316] Examples of silicone surfactants, hydrocarbon surfactants, nonionic surfactants, cationic surfactants, and anionic surfactants include the compounds described in paragraphs 0329 to 0334 of WO 2021 / 112189, the contents of which are incorporated herein by reference.
[0317] The surfactant may be used alone or in combination of two or more. The content of the surfactant is preferably 0.001 to 2.0 mass %, more preferably 0.005 to 1.0 mass %, based on the total solid content of the composition.
[0318] [Higher Fatty Acid Derivative] In order to prevent polymerization inhibition caused by oxygen, a higher fatty acid derivative such as behenic acid or behenic acid amide may be added to the resin composition of the present invention, and the higher fatty acid derivative may be unevenly distributed on the surface of the resin composition of the present invention during drying after application.
[0319] In addition, the higher fatty acid derivative may be a compound described in paragraph 0155 of WO 2015 / 199219, the contents of which are incorporated herein by reference.
[0320] When the resin composition contains a higher fatty acid derivative, the content of the higher fatty acid derivative is preferably 0.1 to 10 mass% based on the total solid content of the resin composition. Only one type of higher fatty acid derivative may be used, or two or more types may be used. When two or more types of higher fatty acid derivatives are used, the total content thereof is preferably within the above range.
[0321] [Thermal Polymerization Initiator] Examples of thermal polymerization initiators include thermal radical polymerization initiators. Thermal radical polymerization initiators are compounds that generate radicals by thermal energy and initiate or promote the polymerization reaction of a polymerizable compound. Addition of a thermal radical polymerization initiator can also promote the polymerization reaction of the resin and the polymerizable compound, thereby further improving solvent resistance. In addition, photopolymerization initiators may also have the function of initiating polymerization by heat, and may be added as a thermal polymerization initiator.
[0322] Specific examples of the thermal radical polymerization initiator include compounds described in paragraphs 0074 to 0118 of JP-A-2008-063554, the contents of which are incorporated herein by reference.
[0323] When a thermal polymerization initiator is contained, the content thereof is preferably 0.1 to 30 mass% relative to the total solid content of the resin composition, more preferably 0.1 to 20 mass%, and even more preferably 0.5 to 15 mass%. Only one type of thermal polymerization initiator may be contained, or two or more types may be contained. When two or more types of thermal polymerization initiators are contained, it is preferable that the total amount is in the above range.
[0324] [Inorganic Particles] Specific examples of inorganic particles include calcium carbonate, calcium phosphate, silica, kaolin, talc, titanium dioxide, alumina, barium sulfate, calcium fluoride, lithium fluoride, zeolite, molybdenum sulfide, and glass.
[0325] The average particle size of the inorganic particles is preferably 0.01 to 2.0 μm, more preferably 0.02 to 1.5 μm, even more preferably 0.03 to 1.0 μm, and particularly preferably 0.04 to 0.5 μm. The above average particle size of the inorganic particles is the primary particle size and also the volume average particle size. The volume average particle size can be measured, for example, by dynamic light scattering using a Nanotrac WAVE II EX-150 (manufactured by Nikkiso Co., Ltd.). If the above measurement is difficult, it can also be measured by centrifugal sedimentation light transmission method, X-ray transmission method, or laser diffraction / scattering method.
[0326] [Ultraviolet absorber] Examples of the ultraviolet absorber include salicylate-based, benzophenone-based, benzotriazole-based, substituted acrylonitrile-based, triazine-based, etc. Specific examples of the ultraviolet absorber include the compounds described in paragraphs 0341 to 0342 of WO 2021 / 112189, the contents of which are incorporated herein by reference.
[0327] The ultraviolet absorbers may be used singly or in combination of two or more. When the resin composition contains an ultraviolet absorber, the content of the ultraviolet absorber is preferably 0.001% by mass or more and 1% by mass or less, and more preferably 0.01% by mass or more and 0.1% by mass or less, based on the total solid mass of the resin composition.
[0328] [Organotitanium Compound] When the resin composition contains an organotitanium compound, a resin layer having excellent chemical resistance can be formed even when cured at low temperatures.
[0329] Usable organic titanium compounds include those in which an organic group is bonded to a titanium atom via a covalent bond or an ionic bond. Specific examples of organic titanium compounds are shown below in I) to VII): I) Titanium chelate compounds: Titanium chelate compounds having two or more alkoxy groups are more preferred because they provide good storage stability to the resin composition and a good curing pattern. Specific examples include titanium bis(triethanolamine) diisopropoxide, titanium di(n-butoxide) bis(2,4-pentanedionate), titanium diisopropoxide bis(2,4-pentanedionate), titanium diisopropoxide bis(tetramethylheptanedionate), and titanium diisopropoxide bis(ethylacetoacetate). II) Tetraalkoxytitanium compounds: for example, titanium tetra(n-butoxide), titanium tetraethoxide, titanium tetra(2-ethylhexoxide), titanium tetraisobutoxide, titanium tetraisopropoxide, titanium tetramethoxide, titanium tetramethoxypropoxide, titanium tetramethylphenoxide, titanium tetra(n-nonyloxide), titanium tetra(n-propoxide), titanium tetrastearyloxide, titanium tetrakis[bis{2,2-(allyloxymethyl)butoxide}], etc. III) Titanocene compounds: for example, pentamethylcyclopentadienyltitanium trimethoxide, bis(η5-2,4-cyclopentadien-1-yl)bis(2,6-difluorophenyl)titanium, bis(η5-2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, etc. IV) Monoalkoxytitanium compounds: for example, titanium tris(dioctylphosphate)isopropoxide, titanium tris(dodecylbenzenesulfonate)isopropoxide, etc. V) Titanium oxide compounds: for example, titanium oxide bis(pentanedionate), titanium oxide bis(tetramethylheptanedionate), phthalocyanine titanium oxide, etc.VI) Titanium tetraacetylacetonate compounds: For example, titanium tetraacetylacetonate, etc. VII) Titanate coupling agents: For example, isopropyl tridodecylbenzenesulfonyl titanate, etc.
[0330] Among these, from the viewpoint of better chemical resistance, the organic titanium compound is preferably at least one compound selected from the group consisting of I) titanium chelate compounds, II) tetraalkoxytitanium compounds, and III) titanocene compounds. In particular, titanium diisopropoxide bis(ethylacetoacetate), titanium tetra(n-butoxide), and bis(η5-2,4-cyclopentadien-1-yl)bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium are preferred.
[0331] When an organotitanium compound is contained, its content is preferably 0.05 to 10 parts by mass, and more preferably 0.1 to 2 parts by mass, relative to 100 parts by mass of the specific resin. When the content is 0.05 part by mass or more, the heat resistance and chemical resistance of the obtained cured pattern are improved, and when it is 10 parts by mass or less, the storage stability of the composition is superior.
[0332] [Antioxidant] By including an antioxidant as an additive, the elongation properties of the cured film and adhesion to metal materials can be improved. Examples of antioxidants include phenol compounds, phosphite ester compounds, and thioether compounds. Specific examples of antioxidants include the compounds described in paragraphs 0348 to 0357 of WO 2021 / 112189, the contents of which are incorporated herein by reference.
[0333] The content of the antioxidant is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the specific resin. By adding an amount of 0.1 part by mass or more, it is easy to obtain the effect of improving elongation properties and adhesion to metal materials even in high-temperature, high-humidity environments, and by adding an amount of 10 parts by mass or less, the sensitivity of the resin composition is improved. Only one type of antioxidant may be used, or two or more types may be used. When two or more types are used, it is preferable that the total amount thereof be within the above range.
[0334] [Anti-aggregating Agent] Examples of the anti-aggregating agent include sodium polyacrylate.
[0335] The anti-aggregating agent may be used singly or in combination of two or more. When the resin composition contains an anti-aggregating agent, the content of the anti-aggregating agent is preferably 0.01 mass % or more and 10 mass % or less, and more preferably 0.02 mass % or more and 5 mass % or less, relative to the total mass of the solid content of the resin composition.
[0336] [Phenol-based compounds] Examples of phenol-based compounds include Bis-Z, BisP-EZ, TekP-4HBPA, TrisP-HAP, TrisP-PA, BisOCHP-Z, BisP-MZ, BisP-PZ, BisP-IPZ, BisOCP-IPZ, BisP-CP, BisRS-2P, BisRS-3P, BisP-OCHP, Methylenetrith-FR-CR, and BisRS-26X (all trade names, manufactured by Honshu Chemical Industry Co., Ltd.), BIP-PC, BIR-PC, BIR-PTBP, and BIR-BIPC-F (all trade names, manufactured by Asahi Organic Chemicals Co., Ltd.).
[0337] The phenolic compound may be used alone or in combination of two or more. When the resin composition contains a phenolic compound, the content of the phenolic compound is preferably 0.01% by mass or more and 30% by mass or less, and more preferably 0.02% by mass or more and 20% by mass or less, based on the total solid mass of the resin composition.
[0338] [Other Polymer Compounds] Examples of other polymer compounds include siloxane resins, (meth)acrylic polymers copolymerized with (meth)acrylic acid, novolac resins, resol resins, polyhydroxystyrene resins, and copolymers thereof. The other polymer compounds may be modified compounds into which crosslinking groups such as methylol groups, alkoxymethyl groups, and epoxy groups have been introduced.
[0339] The other polymer compounds may be used singly or in combination of two or more. When the resin composition contains the other polymer compounds, the content of the other polymer compounds is preferably 0.01% by mass or more and 30% by mass or less, and more preferably 0.02% by mass or more and 20% by mass or less, based on the total solid mass of the resin composition.
[0340] <Characteristics of Resin Composition> The viscosity of the resin composition of the present invention can be adjusted by the solid content concentration of the resin composition. 2 / s~12,000mm 2 / s is preferred, and 2,000 mm 2 / s~10,000mm 2 / s is more preferable, and 2,500 mm 2 / s~8,000mm 2 Within the above range, it is easy to obtain a highly uniform coating film. 2 If the thickness is more than 12,000 mm / s, it is easy to apply the coating to a thickness required for an insulating film for rewiring, for example. 2 If the viscosity is 1 / s or less, a coating film having excellent coating surface condition can be obtained.
[0341] <Restrictions on substances contained in the resin composition> The water content of the resin composition of the present invention is preferably less than 2.0% by mass, more preferably less than 1.5% by mass, and even more preferably less than 1.0% by mass. If it is less than 2.0%, the storage stability of the resin composition is improved. Methods for maintaining the water content include adjusting the humidity under storage conditions and reducing the porosity of the storage container during storage.
[0342] From the viewpoint of insulating properties, the metal content of the resin composition of the present invention is preferably less than 5 mass ppm (parts per million), more preferably less than 1 mass ppm, and even more preferably less than 0.5 mass ppm. Examples of metals include sodium, potassium, magnesium, calcium, iron, copper, chromium, and nickel, but metals contained as complexes of organic compounds and metals are excluded. When multiple metals are contained, the total amount of these metals is preferably within the above range.
[0343] Furthermore, examples of methods for reducing metal impurities unintentionally contained in the resin composition of the present invention include selecting raw materials with a low metal content as raw materials for constituting the resin composition of the present invention, filtering the raw materials for constituting the resin composition of the present invention, and lining the inside of the apparatus with polytetrafluoroethylene or the like to perform distillation under conditions that minimize contamination as much as possible.
[0344] Considering the use of the resin composition of the present invention as a semiconductor material, the content of halogen atoms is preferably less than 500 ppm by mass, more preferably less than 300 ppm by mass, and even more preferably less than 200 ppm by mass, from the viewpoint of wiring corrosion. In particular, those present in the form of halogen ions are preferably less than 5 ppm by mass, more preferably less than 1 ppm by mass, and even more preferably less than 0.5 ppm by mass. Examples of halogen atoms include chlorine atoms and bromine atoms. It is preferable that the total of chlorine atoms and bromine atoms, or chlorine ions and bromine ions, is within the above-mentioned range. Preferred methods for adjusting the content of halogen atoms include ion exchange treatment.
[0345] A conventionally known container can be used as a container for storing the resin composition of the present invention. For the purpose of preventing impurities from being mixed into the raw materials or the resin composition of the present invention, it is also preferable to use a multi-layer bottle whose inner wall is made of six types of six resin layers, or a bottle with a seven-layer structure made of six types of resin. Examples of such containers include the container described in JP 2015-123351 A.
[0346] <Cured Product of Resin Composition> A cured product of the resin composition can be obtained by curing the resin composition of the present invention. The cured product of the present invention is a cured product obtained by curing the resin composition. The resin composition is preferably cured by heating, with a heating temperature of 120°C to 400°C being more preferred, 140°C to 380°C being even more preferred, and 170°C to 350°C being particularly preferred. The form of the cured product of the resin composition is not particularly limited, and can be selected depending on the application, such as a film, rod, sphere, or pellet. In the present invention, the cured product is preferably in the form of a film. By patterning the resin composition, the shape of the cured product can be selected depending on the application, such as forming a protective film on a wall surface, forming via holes for electrical conductivity, adjusting impedance, capacitance, or internal stress, or imparting heat dissipation functionality. The film thickness of the cured product (film made of the cured product) is preferably 0.5 μm or more and 150 μm or less. The shrinkage rate when the resin composition of the present invention is cured is preferably 50% or less, more preferably 45% or less, and even more preferably 40% or less. Here, the shrinkage rate refers to the percentage of change in volume of the resin composition before and after curing, and can be calculated by the following formula: Shrinkage rate [%] = 100 - (volume after curing / volume before curing) x 100
[0347] <Characteristics of cured product of resin composition> The imidization reaction rate of the cured product of the resin composition of the present invention is preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more. If it is 70% or more, the cured product may have excellent mechanical properties. The elongation at break of the cured product of the resin composition of the present invention is preferably 30% or more, more preferably 40% or more, and even more preferably 50% or more. The glass transition temperature (Tg) of the cured product of the resin composition of the present invention is preferably 180°C or more, more preferably 210°C or more, and even more preferably 230°C or more.
[0348] <Preparation of Resin Composition> The resin composition of the present invention can be prepared by mixing the above-mentioned components. The mixing method is not particularly limited, and can be carried out by a conventionally known method. Examples of the mixing method include mixing with a stirring blade, mixing with a ball mill, and mixing by rotating a tank. The temperature during mixing is preferably 10 to 30°C, more preferably 15 to 25°C.
[0349] Filtration using a filter is preferably performed to remove foreign matter such as dust and fine particles from the resin composition of the present invention. The filter pore size is, for example, preferably 5 μm or less, more preferably 1 μm or less, even more preferably 0.5 μm or less, and even more preferably 0.1 μm or less. The filter material is preferably polytetrafluoroethylene, polyethylene, or nylon. When the filter material is polyethylene, HDPE (high-density polyethylene) is more preferable. The filter may be pre-washed with an organic solvent. In the filter filtration process, multiple types of filters may be connected in series or parallel. When multiple types of filters are used, filters with different pore sizes or materials may be combined. An example of a connection mode is a mode in which an HDPE filter with a pore size of 1 μm is connected in series as the first stage and an HDPE filter with a pore size of 0.2 μm is connected in series as the second stage. Various materials may also be filtered multiple times. When filtration is performed multiple times, circulating filtration may be used. Filtration may also be performed under pressure. When filtering under pressure, the pressure to be applied is preferably 0.01 MPa or more and 1.0 MPa or less, more preferably 0.03 MPa or more and 0.9 MPa or less, even more preferably 0.05 MPa or more and 0.7 MPa or less, and even more preferably 0.05 MPa or more and 0.5 MPa or less. In addition to filtering using a filter, a process of removing impurities using an adsorbent may be performed. Filter filtration and a process of removing impurities using an adsorbent may be combined. Known adsorbents can be used as the adsorbent. Examples include inorganic adsorbents such as silica gel and zeolite, and organic adsorbents such as activated carbon. After filtering using a filter, the resin composition filled in a bottle may be subjected to a degassing process by placing it under reduced pressure.
[0350] <Method for Producing a Cured Product> The method for producing a cured product of the present invention preferably includes a film-forming step of applying a resin composition to a substrate to form a film (preferably a photosensitive film). The method for producing a cured product more preferably includes the film-forming step, an exposure step of exposing (preferably selectively exposing) the film formed in the film-forming step, and a development step of developing the film exposed in the exposure step (exposed film) with a developer to form a pattern (preferably an insulating pattern). The method for producing a cured product particularly preferably includes the film-forming step, the exposure step, the development step, and at least one of a heating step of heating the pattern obtained in the development step and a post-development exposure step of exposing the pattern obtained in the development step. The method for producing a cured product also preferably includes the film-forming step and a step of heating the film. Details of each step are described below.
[0351] (Film Forming Step) The resin composition of the present invention can be used in a film forming step of applying the resin composition to a substrate to form a film. The method for producing a cured product of the present invention preferably includes a film forming step of applying the resin composition to a substrate to form a film.
[0352] [Substrate] The type of substrate can be appropriately determined depending on the application and is not particularly limited. Examples of substrates include semiconductor production substrates such as silicon, silicon nitride, polysilicon, silicon oxide, and amorphous silicon, quartz, glass, optical films, ceramic materials, vapor deposition films, magnetic films, reflective films, metal substrates such as Ni, Cu, Cr, and Fe (for example, substrates formed from metal and substrates on which a metal layer is formed by, for example, plating or vapor deposition), paper, SOG (Spin On Glass), TFT (Thin Film Transistor) array substrates, mold substrates, and plasma display panel (PDP) electrode plates. Substrates are particularly preferably semiconductor production substrates, with silicon substrates, Cu substrates, and mold substrates being more preferred. These substrates may have a surface layer such as an adhesion layer or an oxide layer formed by hexamethyldisilazane (HMDS) or the like. The shape of the substrate is not particularly limited and may be circular or rectangular. The size of the substrate is preferably, for example, a diameter of 100 to 450 mm, more preferably 200 to 450 mm, if it is circular. If it is rectangular, the length of the short side is preferably, for example, 100 to 1000 mm, more preferably 200 to 700 mm. As the substrate, for example, a plate-shaped, preferably a panel-shaped substrate (substrate) is used.
[0353] When a film is formed by applying a resin composition to the surface of a resin layer (for example, a layer made of a cured product) or the surface of a metal layer, the resin layer or the metal layer serves as the substrate.
[0354] Coating is preferred as a means for applying the resin composition to a substrate. Specific application methods include dip coating, air knife coating, curtain coating, wire bar coating, gravure coating, extrusion coating, spray coating, spin coating, slit coating, and inkjet coating. From the viewpoint of uniformity of film thickness, spin coating, slit coating, spray coating, or inkjet coating is preferred, and from the viewpoint of uniformity of film thickness and productivity, spin coating and slit coating are more preferred. By adjusting the solid content concentration of the resin composition and coating conditions depending on the application method, a film of the desired thickness can be obtained. In addition, the coating method can be appropriately selected depending on the shape of the substrate. For circular substrates such as wafers, spin coating, spray coating, inkjet coating, etc. are preferred, and for rectangular substrates, slit coating, spray coating, inkjet coating, etc. are preferred. In the case of spin coating, for example, it can be applied at a rotation speed of 500 to 3,500 rpm for about 10 seconds to 3 minutes. Alternatively, a method can be used in which a coating film formed by applying the coating composition to a temporary support in advance using the above-described application method is transferred onto the substrate. Regarding the transfer method, the preparation methods described in paragraphs 0023 and 0036 to 0051 of JP-A No. 2006-023696 and paragraphs 0096 to 0108 of JP-A No. 2006-047592 can be suitably used. A step of removing excess film from the edge of the substrate may also be performed. Examples of such a step include edge bead rinsing (EBR) and back rinsing. A pre-wetting step may also be employed in which the substrate is coated with various solvents before applying the resin composition to the substrate, improving the wettability of the substrate and then applying the resin composition.
[0355] (Drying Step) After the film-forming step (layer-forming step), the film may be subjected to a step (drying step) of drying the formed film (layer) to remove the solvent. That is, the method for producing a cured product of the present invention may include a drying step of drying the film formed in the film-forming step. The drying step is preferably carried out after the film-forming step and before the exposure step. The drying temperature of the film in the drying step is preferably 50 to 150°C, more preferably 70 to 130°C, and even more preferably 90 to 110°C. Drying may also be carried out under reduced pressure. The drying time is, for example, 30 seconds to 20 minutes, preferably 1 to 10 minutes, and more preferably 2 to 7 minutes.
[0356] (Exposure Step) The above-mentioned film may be subjected to an exposure step in which the film is selectively exposed to light. The method for producing a cured product may include an exposure step in which the film formed in the film formation step is selectively exposed to light. Selective exposure means that a portion of the film is exposed to light. Furthermore, selective exposure forms exposed regions (exposed portions) and unexposed regions (unexposed portions) in the film. The exposure dose is not particularly limited as long as it can cure the resin composition of the present invention, but for example, it is 50 to 10,000 mJ / cm in terms of exposure energy at a wavelength of 365 nm. 2 is preferred, and 200 to 8,000 mJ / cm 2 is more preferred.
[0357] The exposure wavelength can be appropriately determined within the range of 190 to 1,000 nm, and is preferably 240 to 550 nm.
[0358] The exposure wavelengths, in relation to the light source, are: (1) semiconductor laser (wavelengths 830 nm, 532 nm, 488 nm, 405 nm, 375 nm, 355 nm, etc.); (2) metal halide lamp; (3) high-pressure mercury lamp, g-line (wavelength 436 nm), h-line (wavelength 405 nm), i-line (wavelength 365 nm), broad (three wavelengths of g, h, and i-line); (4) excimer laser, KrF excimer laser (wavelength 248 nm), ArF excimer laser (wavelength 193 nm), F 2Examples of such light include excimer laser (wavelength 157 nm), (5) extreme ultraviolet light; EUV (wavelength 13.6 nm), (6) electron beam, and (7) YAG laser second harmonic 532 nm and third harmonic 355 nm. For the resin composition of the present invention, exposure with a high-pressure mercury lamp is particularly preferred, and exposure with i-line is more preferred from the viewpoint of exposure sensitivity. The exposure method is not particularly limited as long as it is a method that exposes at least a portion of the film made of the resin composition of the present invention, and examples thereof include exposure using a photomask and exposure by laser direct imaging.
[0359] (Post-exposure baking step) The film may be subjected to a heating step (post-exposure baking step) after exposure. That is, the method for producing a cured product of the present invention may include a post-exposure baking step in which the film exposed in the exposure step is heated. The post-exposure baking step can be carried out after the exposure step and before the development step. The heating temperature in the post-exposure baking step is preferably 40 to 160°C, more preferably 50 to 140°C, and even more preferably 60 to 120°C. The heating time in the post-exposure baking step is preferably 30 seconds to 300 minutes, and more preferably 1 to 10 minutes. The temperature rise rate in the post-exposure baking step from the temperature at the start of heating to the maximum heating temperature is preferably 1 to 12°C / min, more preferably 2 to 10°C / min, and even more preferably 3 to 10°C / min. The temperature rise rate may also be changed as appropriate during heating. The heating means in the post-exposure baking step is not particularly limited, and known hot plates, ovens, infrared heaters, etc. may be used. It is also preferable to carry out the heating in an atmosphere of low oxygen concentration by flowing an inert gas such as nitrogen, helium, or argon.
[0360] (Development step) The film after exposure may be subjected to a development step in which it is developed using a developer to form a pattern. That is, the method for producing a cured product of the present invention may include a development step in which the film exposed in the exposure step is developed using a developer to form a pattern. By carrying out development, one of the exposed and unexposed parts of the film is removed to form a pattern. Here, development in which the unexposed parts of the film are removed in the development step is called negative development, and development in which the exposed parts of the film are removed in the development step is called positive development.
[0361] [Developer] The developer used in the development step includes an aqueous solution (preferably water or an alkaline aqueous solution) or a developer containing an organic solvent.
[0362] When the developer is water, pure water such as ion-exchanged water, distilled water, or RO (reverse osmosis) water, or ultrapure water obtained by irradiating such pure water with UV light or filtering through a UF (ultrafiltration) membrane may be used. When the developer is an alkaline aqueous solution, examples of the basic compound that can be contained in the alkaline aqueous solution include inorganic alkalis, primary amines, secondary amines, tertiary amines, and quaternary ammonium salts. Preferred are TMAH (tetramethylammonium hydroxide), potassium hydroxide, sodium carbonate, sodium hydroxide, sodium silicate, sodium metasilicate, ammonia, ethylamine, n-propylamine, diethylamine, di-n-butylamine, triethylamine, methyldiethylamine, dimethylethanolamine, triethanolamine, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, tetrapentylammonium hydroxide, tetrahexylammonium hydroxide, tetraoctylammonium hydroxide, ethyltrimethylammonium hydroxide, butyltrimethylammonium hydroxide, methyltriamylammonium hydroxide, dibutyldipentylammonium hydroxide, dimethylbis(2-hydroxyethyl)ammonium hydroxide, trimethylphenylammonium hydroxide, trimethylbenzylammonium hydroxide, triethylbenzylammonium hydroxide, pyrrole, and piperidine, and more preferred is TMAH. The content of the basic compound in the developer is preferably from 0.01 to 10% by mass, more preferably from 0.1 to 5% by mass, and even more preferably from 0.3 to 3% by mass, based on the total mass of the developer.
[0363] When the developer contains an organic solvent, the organic solvent may be a compound described in paragraph
[0387] of WO 2021 / 112189, the contents of which are incorporated herein by reference. Suitable examples of alcohols include methanol, ethanol, propanol, isopropanol, butanol, pentanol, octanol, diethylene glycol, propylene glycol, methyl isobutyl carbinol, and triethylene glycol, and suitable examples of amides include N-methylpyrrolidone, N-ethylpyrrolidone, and dimethylformamide.
[0364] When the developer contains an organic solvent, the organic solvent may be used alone or in combination. In the present invention, a developer containing at least one selected from the group consisting of cyclopentanone, γ-butyrolactone, dimethyl sulfoxide, N-methyl-2-pyrrolidone, and cyclohexanone is particularly preferred, a developer containing at least one selected from the group consisting of cyclopentanone, γ-butyrolactone, and dimethyl sulfoxide is more preferred, and a developer containing cyclopentanone is particularly preferred.
[0365] When the developer contains an organic solvent, the content of the organic solvent relative to the total mass of the developer is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more. Alternatively, the content may be 100% by mass.
[0366] When the developer contains an organic solvent, the developer may further contain at least one of a basic compound and a base generator. When at least one of the basic compound and the base generator in the developer permeates into the pattern, the performance of the pattern, such as breaking elongation, may be improved.
[0367] As the basic compound, from the viewpoint of reliability when it remains in the film after curing (adhesion to the substrate when the cured product is further heated), an organic base is preferred. As the basic compound, a basic compound having an amino group is preferred, and primary amines, secondary amines, tertiary amines, ammonium salts, tertiary amides, etc. are preferred. However, to promote the imidization reaction, primary amines, secondary amines, tertiary amines, or ammonium salts are preferred, secondary amines, tertiary amines, or ammonium salts are more preferred, secondary amines or tertiary amines are even more preferred, and tertiary amines are particularly preferred. As the basic compound, from the viewpoint of the mechanical properties (elongation at break) of the cured product, it is preferred that it is difficult for the amount remaining to decrease before heating due to vaporization, etc., is preferred. Therefore, the boiling point of the basic compound is preferably 30°C to 350°C at normal pressure (101,325 Pa), more preferably 80°C to 270°C, and even more preferably 100°C to 230°C. The boiling point of the basic compound is preferably higher than the temperature obtained by subtracting 20° C. from the boiling point of the organic solvent contained in the developer, and more preferably higher than the boiling point of the organic solvent contained in the developer. For example, when the boiling point of the organic solvent is 100° C., the boiling point of the basic compound used is preferably 80° C. or higher, and more preferably 100° C. or higher. The developer may contain only one type of basic compound, or may contain two or more types.
[0368] Specific examples of the basic compound include ethanolamine, diethanolamine, triethanolamine, ethylamine, diethylamine, triethylamine, hexylamine, dodecylamine, cyclohexylamine, cyclohexylmethylamine, cyclohexyldimethylamine, aniline, N-methylaniline, N,N-dimethylaniline, diphenylamine, pyridine, butylamine, isobutylamine, dibutylamine, tributylamine, dicyclohexylamine, DBU (diazabicycloundecene), DABCO (1,4-diazabicyclo[2.2.2]octane), N,N-diisopropylethylamine, tetramethylammonium hydroxide, tetrabutylammonium hydroxide, ethylenediamine, butanediamine, 1,5-diamino Examples of the alkyl ester include pentane, N-methylhexylamine, N-methyldicyclohexylamine, trioctylamine, N-ethylethylenediamine, N,N-diethylethylenediamine, N,N,N',N'-tetrabutyl-1,6-hexanediamine, spermidine, diaminocyclohexane, bis(2-methoxyethyl)amine, piperidine, methylpiperidine, dimethylpiperidine, piperazine, tropane, N-phenylbenzylamine, 1,2-dianilinoethane, 2-aminoethanol, toluidine, aminophenol, hexylaniline, phenylenediamine, phenylethylamine, dibenzylamine, pyrrole, N-methylpyrrole, N,N,N,N-tetramethylethylenediamine, and N,N,N,N-tetramethyl-1,3-propanediamine.
[0369] The preferred embodiments of the base generator are the same as those of the base generator contained in the composition described above. In particular, the base generator is preferably a thermal base generator.
[0370] When the developer contains at least one of a basic compound and a base generator, the content of the basic compound or base generator is preferably 10% by mass or less, more preferably 5% by mass or less, based on the total mass of the developer. The lower limit of the content is not particularly limited, but is preferably, for example, 0.1% by mass or more. When the basic compound or base generator is solid in the environment in which the developer is used, the content of the basic compound or base generator is also preferably 70 to 100% by mass, based on the total solid content of the developer. The developer may contain only one type of basic compound or base generator, or two or more types. When two or more types of at least one of the basic compound and base generator are used, the total content thereof is preferably within the above-mentioned range.
[0371] The developer may further contain other components, such as known surfactants and known defoaming agents.
[0372] [Method of Supplying Developer] The method of supplying the developer is not particularly limited as long as it can form the desired pattern, and includes a method of immersing a substrate on which a film has been formed in the developer, puddle development in which the developer is supplied to the film formed on the substrate using a nozzle, and a method of continuously supplying the developer. The type of nozzle is not particularly limited, and examples include a straight nozzle, a shower nozzle, and a spray nozzle. From the viewpoints of the permeability of the developer, the removability of non-image areas, and production efficiency, a method of supplying the developer using a straight nozzle or a method of continuously supplying the developer using a spray nozzle is preferred, and from the viewpoint of the permeability of the developer to the image areas, a method of supplying using a spray nozzle is more preferred. In addition, a process may be adopted in which the developer is continuously supplied using a straight nozzle, the substrate is spun to remove the developer from the substrate, and after spin drying, the developer is continuously supplied again using a straight nozzle, and the substrate is spun to remove the developer from the substrate, or this process may be repeated multiple times. Methods of supplying the developer in the development process include a process in which the developer is continuously supplied to the substrate, a process in which the developer is kept substantially stationary on the substrate, a process in which the developer is vibrated on the substrate using ultrasound or the like, and a combination thereof.
[0373] The development time is preferably 10 seconds to 10 minutes, more preferably 20 seconds to 5 minutes. The temperature of the developer during development is not particularly limited, but is preferably 10 to 45°C, more preferably 18 to 30°C.
[0374] In the developing step, after the treatment with the developer, the pattern may be further washed (rinsed) with a rinse liquid. Alternatively, a method may be employed in which a rinse liquid is supplied before the developer in contact with the pattern is completely dried.
[0375] [Rinse Liquid] When the developer is water, for example, water can be used as the rinse liquid. When the developer is an alkaline aqueous solution, for example, water can be used as the rinse liquid. When the developer is a developer containing an organic solvent, for example, a solvent different from the solvent contained in the developer (for example, water, an organic solvent different from the organic solvent contained in the developer) can be used as the rinse liquid.
[0376] When the rinse solution contains an organic solvent, examples of the organic solvent include the same organic solvents as those exemplified when the developer contains an organic solvent. The organic solvent contained in the rinse solution is preferably different from the organic solvent contained in the developer, and more preferably an organic solvent that has a lower solubility for the pattern than the organic solvent contained in the developer.
[0377] When the rinse solution contains an organic solvent, the organic solvent may be used alone or in combination of two or more. The organic solvent is preferably cyclopentanone, γ-butyrolactone, dimethyl sulfoxide, N-methylpyrrolidone, cyclohexanone, propylene glycol monomethyl ether acetate (PGMEA), or propylene glycol monomethyl ether (PGME), more preferably cyclopentanone, γ-butyrolactone, dimethyl sulfoxide, PGMEA, or PGME, and even more preferably cyclohexanone or PGMEA.
[0378] When the rinse solution contains an organic solvent, the organic solvent preferably accounts for 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more of the total mass of the rinse solution, and may also account for 100% by mass of the total mass of the rinse solution.
[0379] The rinse solution may contain at least one of a basic compound and a base generator. Although not particularly limited, when the developer contains an organic solvent, an embodiment in which the rinse solution contains the organic solvent and at least one of a basic compound and a base generator is also one of the preferred embodiments of the present invention. Examples of the basic compound and base generator contained in the rinse solution include the compounds exemplified as the basic compound and base generator that may be contained when the developer contains an organic solvent, and the same applies to preferred embodiments. The basic compound and base generator contained in the rinse solution may be selected taking into consideration the solubility in the solvent in the rinse solution, etc.
[0380] When the rinse solution contains at least one of a basic compound and a base generator, the content of the basic compound or base generator is preferably 10% by mass or less, and more preferably 5% by mass or less, based on the total mass of the rinse solution. The lower limit of the content is not particularly limited, but is preferably 0.1% by mass or more, for example. When the basic compound or base generator is solid in the environment in which the rinse solution is used, the content of the basic compound or base generator is also preferably 70 to 100% by mass, based on the total solid content of the rinse solution. When the rinse solution contains at least one of a basic compound and a base generator, the rinse solution may contain only one type of at least one of the basic compound and the base generator, or may contain two or more types. When at least one of the basic compound and the base generator is two or more types, the total content thereof is preferably within the above-mentioned range.
[0381] The rinse liquid may further contain other components, such as known surfactants and known defoaming agents.
[0382] [Method of Supplying Rinse Liquid] The method of supplying the rinse liquid is not particularly limited as long as it can form a desired pattern, and examples thereof include a method of immersing the substrate in the rinse liquid, a method of supplying the rinse liquid to the substrate by puddling, a method of supplying the rinse liquid to the substrate by showering, and a method of continuously supplying the rinse liquid onto the substrate by means of a straight nozzle or the like. From the viewpoints of the permeability of the rinse liquid, the removability of non-image areas, and production efficiency, methods of supplying the rinse liquid using a shower nozzle, straight nozzle, spray nozzle, etc. are available, and a method of continuously supplying using a spray nozzle is preferred, and from the viewpoint of the permeability of the rinse liquid into the image areas, a method of supplying using a spray nozzle is more preferred. The type of nozzle is not particularly limited, and examples include a straight nozzle, shower nozzle, spray nozzle, etc. That is, the rinsing step is preferably a step of supplying or continuously supplying the rinse liquid to the exposed film using a straight nozzle, and more preferably a step of supplying the rinse liquid using a spray nozzle. The method of supplying the rinse liquid in the rinsing step may include a step of continuously supplying the rinse liquid to the substrate, a step of keeping the rinse liquid substantially stationary on the substrate, a step of vibrating the rinse liquid on the substrate by ultrasonic waves or the like, and a combination of these steps.
[0383] The rinsing time is preferably 10 seconds to 10 minutes, more preferably 20 seconds to 5 minutes. The temperature of the rinsing liquid during rinsing is not particularly limited, but is preferably 10 to 45°C, more preferably 18 to 30°C.
[0384] The developing step may include a step of contacting the pattern with a treatment liquid after treatment with a developer or after washing the pattern with a rinse liquid. Alternatively, a method may be employed in which the treatment liquid is supplied before the developer or rinse liquid in contact with the pattern is completely dried.
[0385] The treatment liquid may include a treatment liquid containing at least one of water and an organic solvent, and at least one of a basic compound and a base generator. Preferred aspects of the organic solvent, the basic compound, and the base generator are the same as the preferred aspects of the organic solvent, the basic compound, and the base generator used in the rinse liquid described above. The treatment liquid can be supplied to the pattern using the same method as the rinse liquid described above, and preferred aspects are also the same.
[0386] The content of the basic compound or base generator in the treatment liquid is preferably 10% by mass or less, and more preferably 5% by mass or less, relative to the total mass of the treatment liquid. There is no particular limitation on the lower limit of the content, but it is preferably, for example, 0.1% by mass or more. Furthermore, when the basic compound or base generator is solid in the environment in which the treatment liquid is used, the content of the basic compound or base generator is also preferably 70 to 100% by mass, relative to the total solid content of the treatment liquid. When the treatment liquid contains at least one of a basic compound and a base generator, the treatment liquid may contain only one type of at least one of the basic compound and the base generator, or may contain two or more types. When there are two or more types of at least one of the basic compound and the base generator, it is preferable that the total amount thereof is within the above-mentioned range.
[0387] (Heating Step) The pattern obtained in the development step (or the pattern after rinsing, if a rinsing step is performed) may be subjected to a heating step in which the pattern obtained by the development step is heated. That is, the method for producing a cured product of the present invention may include a heating step in which the pattern obtained in the development step is heated. Furthermore, the method for producing a cured product of the present invention may include a heating step in which a pattern obtained by another method without performing a development step, or a film obtained in the film formation step is heated. In the heating step, a resin such as a polyimide precursor is cyclized to form a resin such as a polyimide. Furthermore, crosslinking of unreacted crosslinkable groups in the specific resin or in a crosslinking agent other than the specific resin also proceeds. The heating temperature (maximum heating temperature) in the heating step is preferably 50 to 450°C, more preferably 150 to 350°C, even more preferably 150 to 250°C, even more preferably 160 to 250°C, and particularly preferably 160 to 230°C.
[0388] The heating step is preferably a step in which the cyclization reaction of the polyimide precursor is promoted within the pattern by the action of a base or the like generated from the base generator due to heating.
[0389] The heating step is preferably carried out at a temperature increase rate of 1 to 12°C / min from the temperature at the start of heating to the maximum heating temperature. The temperature increase rate is more preferably 2 to 10°C / min, and even more preferably 3 to 10°C / min. By setting the temperature increase rate to 1°C / min or more, it is possible to prevent excessive volatilization of the acid or solvent while ensuring productivity, and by setting the temperature increase rate to 12°C / min or less, it is possible to alleviate residual stress in the cured product. In addition, in the case of an oven capable of rapid heating, it is preferable to increase the temperature from the temperature at the start of heating to the maximum heating temperature at a temperature increase rate of 1 to 8°C / sec, more preferably 2 to 7°C / sec, and even more preferably 3 to 6°C / sec.
[0390] The temperature at the start of heating is preferably 20°C to 150°C, more preferably 20°C to 130°C, and even more preferably 25°C to 120°C. The temperature at the start of heating refers to the temperature at the start of the process of heating up to the maximum heating temperature. For example, when the resin composition of the present invention is applied to a substrate and then dried, the temperature is the temperature of the film (layer) after this drying, and it is preferable to raise the temperature from, for example, a temperature 30 to 200°C lower than the boiling point of the solvent contained in the resin composition.
[0391] The heating time (heating time at the maximum heating temperature) is preferably from 5 to 360 minutes, more preferably from 10 to 300 minutes, and even more preferably from 15 to 240 minutes.
[0392] In particular, when forming a multilayer laminate, from the viewpoint of interlayer adhesion, the heating temperature is preferably 30° C. or higher, more preferably 80° C. or higher, even more preferably 100° C. or higher, and particularly preferably 120° C. or higher. The upper limit of the heating temperature is preferably 350° C. or lower, more preferably 250° C. or lower, and even more preferably 240° C. or lower.
[0393] Heating may be performed in stages. For example, the temperature may be increased from 25°C to 120°C at a rate of 3°C / min, held at 120°C for 60 minutes, increased from 120°C to 180°C at a rate of 2°C / min, and held at 180°C for 120 minutes. It is also preferable to treat the film while irradiating it with ultraviolet light, as described in U.S. Pat. No. 9,159,547. Such a pretreatment step can improve the film's properties. The pretreatment step is preferably performed for a short period of time, such as 10 seconds to 2 hours, and more preferably 15 seconds to 30 minutes. The pretreatment may be performed in two or more steps. For example, a first pretreatment step may be performed at a temperature in the range of 100 to 150°C, followed by a second pretreatment step at a temperature in the range of 150 to 200°C. Furthermore, cooling may be performed after heating. In this case, the cooling rate is preferably 1 to 5°C / min.
[0394] The heating step is preferably carried out in an atmosphere with a low oxygen concentration by flowing an inert gas such as nitrogen, helium, or argon, or by carrying out the heating step under reduced pressure, in order to prevent decomposition of the specific resin. The oxygen concentration is preferably 50 ppm (volume ratio) or less, more preferably 20 ppm (volume ratio) or less. The heating means used in the heating step is not particularly limited, and examples thereof include a hot plate, an infrared oven, an electric heating oven, a hot air oven, and an infrared oven.
[0395] It should be noted that the specific anions and specific cations in the present invention are hydrophilic, but since they become hydrophobic decomposition products in negative development as described above, and since they are decomposed in the subsequent heating step which is preferably carried out in positive development, they are less likely to remain, which is thought to enable the dielectric loss tangent to be reduced.
[0396] (Post-development exposure step) The pattern obtained in the development step (if a rinsing step is performed, the pattern after rinsing) may be subjected to a post-development exposure step in which the pattern obtained in the development step is exposed to light, instead of or in addition to the heating step. That is, the method for producing a cured product of the present invention may include a post-development exposure step in which the pattern obtained in the development step is exposed to light. The method for producing a cured product of the present invention may include a heating step and a post-development exposure step, or may include only one of the heating step and the post-development exposure step. The post-development exposure step can promote, for example, a reaction in which cyclization of a polyimide precursor or the like progresses due to exposure of a photobase generator, or a reaction in which elimination of an acid-decomposable group progresses due to exposure of a photoacid generator. In the post-development exposure step, it is sufficient that at least a portion of the pattern obtained in the development step is exposed, but it is preferable that the entire pattern is exposed. The exposure dose in the post-development exposure step is 50 to 20,000 mJ / cm in terms of exposure energy at a wavelength to which the photosensitive compound has sensitivity. 2 is preferred, and 100 to 15,000 mJ / cm 2 The post-development exposure step can be carried out using, for example, the light source used in the exposure step described above, and it is preferable to use broadband light.
[0397] (Metal Layer Forming Step) The pattern obtained by the developing step (preferably subjected to at least one of a heating step and a post-development exposure step) may be subjected to a metal layer forming step of forming a metal layer on the pattern. That is, the method for producing a cured product of the present invention preferably includes a metal layer forming step of forming a metal layer on the pattern obtained by the developing step (preferably subjected to at least one of a heating step and a post-development exposure step).
[0398] The metal layer is not particularly limited, and existing metal species can be used. Examples include copper, aluminum, nickel, vanadium, titanium, chromium, cobalt, gold, tungsten, tin, silver, and alloys containing these metals. Copper and aluminum are more preferred, and copper is even more preferred.
[0399] The method for forming the metal layer is not particularly limited, and existing methods can be applied. For example, the methods described in JP 2007-157879 A, JP 2001-521288 A, JP 2004-214501 A, JP 2004-101850 A, U.S. Patent No. 7,888,181 B2, and U.S. Patent No. 9,177,926 B2 can be used. Examples of suitable methods include photolithography, PVD (physical vapor deposition), CVD (chemical vapor deposition), lift-off, electroplating, electroless plating, etching, printing, and combinations of these. More specifically, examples include patterning methods that combine sputtering, photolithography, and etching, and patterning methods that combine photolithography and electroplating. Preferred plating methods include electroplating using a copper sulfate or copper cyanide plating solution.
[0400] The thickness of the metal layer is preferably 0.01 to 50 μm, more preferably 1 to 10 μm, at the thickest part.
[0401] <Applications> Fields to which the method for producing a cured product of the present invention or the cured product can be applied include insulating films for electronic devices, interlayer insulating films for rewiring layers, stress buffer films, etc. Other examples include sealing films, substrate materials (base films, coverlays, and interlayer insulating films for flexible printed circuit boards), and the etching of insulating films for packaging applications such as those described above. For these applications, reference can be made to, for example, Science & Technology Co., Ltd.'s "High Performance Polyimide and Application Technology" (April 2008), edited by Masaaki Kakimoto, CMC Technical Library "Fundamentals and Development of Polyimide Materials" (November 2011), and Japan Polyimide and Aromatic Polymer Research Association's "Latest Polyimide Fundamentals and Applications" (NTS, August 2010).
[0402] The method for producing the cured product of the present invention, or the cured product of the present invention, can also be used for producing printing plates such as offset printing plates or screen printing plates, for etching molded parts, for producing protective lacquers and dielectric layers in electronics, especially microelectronics, etc.
[0403] <Method for manufacturing an interlayer insulating film for a redistribution layer> The method for manufacturing an interlayer insulating film for a redistribution layer of the present invention includes a photosensitive film formation step of applying the resin composition of the present invention to a substrate and forming a photosensitive film, an exposure step of exposing the photosensitive film to light to form an exposed film, and a pattern formation step of developing the exposed film with a developer to form an insulating pattern. In addition to the above steps, the method for manufacturing an interlayer insulating film for a redistribution layer may include at least one of a heating step of heating the insulating pattern obtained by the development step and a post-development exposure step of exposing the insulating pattern obtained by the development step. Furthermore, the method for manufacturing an interlayer insulating film for a redistribution layer may include the photosensitive film formation step and a step of heating the photosensitive film. The above steps are the same as those described in the method for manufacturing a cured product described above. The developer may be an organic solvent or an aqueous solution.
[0404] <Laminate and method for manufacturing laminate> The laminate of the present invention refers to a structure having a plurality of layers each made of the cured product of the present invention. The laminate is a laminate including two or more layers each made of the cured product, and may be a laminate including three or more layers. At least one of the two or more layers each made of the cured product included in the laminate is a layer made of the cured product of the present invention, and from the viewpoint of suppressing shrinkage of the cured product or deformation of the cured product associated with the shrinkage, it is also preferable that all of the layers made of the cured product included in the laminate are layers made of the cured product of the present invention.
[0405] That is, the method for producing a laminate of the present invention preferably includes the method for producing a cured product of the present invention, and more preferably includes repeating the method for producing a cured product of the present invention multiple times.
[0406] The laminate of the present invention preferably includes two or more layers made of a cured product and a metal layer between any of the layers made of the cured product. The metal layer is preferably formed by the metal layer-forming step. That is, the method for producing a laminate of the present invention preferably further includes a metal layer-forming step of forming a metal layer on a layer made of a cured product between multiple cured product production processes. A preferred embodiment of the metal layer-forming step is as described above. Examples of the laminate include a laminate having at least a layer structure in which three layers are stacked in this order: a layer made of a first cured product, a metal layer, and a layer made of a second cured product. It is preferred that both the layer made of the first cured product and the layer made of the second cured product are layers made of the cured product of the present invention. The resin composition of the present invention used to form the layer made of the first cured product and the resin composition of the present invention used to form the layer made of the second cured product may have the same composition or different compositions. The metal layer in the laminate of the present invention is preferably used as metal wiring, such as a rewiring layer.
[0407] (Lamination process) The method for producing a laminate of the present invention preferably includes a lamination process. The lamination process is a series of processes including performing at least one of (a) a film formation process (layer formation process), (b) an exposure process, (c) a development process, and (d) a heating process and a post-development exposure process again on the surface of the pattern (resin layer) or the metal layer in this order. However, at least one of (a) the film formation process and (d) the heating process and the post-development exposure process may be repeated. Furthermore, after at least one of (d) the heating process and the post-development exposure process, (e) a metal layer formation process may be included. It goes without saying that the lamination process may further include the above-mentioned drying process, etc. as appropriate.
[0408] When a further lamination step is performed after the lamination step, a surface activation treatment step may be further performed after the exposure step, the heating step, or the metal layer forming step. An example of the surface activation treatment is a plasma treatment. Details of the surface activation treatment will be described later.
[0409] The lamination step is preferably performed 2 to 20 times, more preferably 2 to 9 times. For example, a structure having 2 to 20 resin layers, such as resin layer / metal layer / resin layer / metal layer / resin layer / metal layer, is preferred, and a structure having 2 to 9 resin layers is even more preferred. Each of the layers may be the same or different in composition, shape, film thickness, etc.
[0410] In the present invention, a particularly preferred embodiment is one in which, after providing a metal layer, a cured product (resin layer) of the resin composition of the present invention is further formed so as to cover the metal layer.Specific examples include an embodiment in which the steps of (a) film formation step, (b) exposure step, (c) development step, (d) at least one of a heating step and a post-development exposure step, and (e) metal layer formation step are repeated in this order, or an embodiment in which the steps of (a) film formation step, (d) at least one of a heating step and a post-development exposure step, and (e) metal layer formation step are repeated in this order.By alternately performing the lamination step of laminating the resin composition layer (resin layer) of the present invention and the metal layer formation step, the resin composition layer (resin layer) of the present invention and the metal layer can be alternately laminated.
[0411] (Surface Activation Treatment Step) The method for producing a laminate of the present invention preferably includes a surface activation treatment step in which at least a portion of the metal layer and the resin composition layer are surface-activated. The surface activation treatment step is usually performed after the metal layer formation step, but after the development step (preferably after at least one of the heating step and the post-development exposure step), the resin composition layer may be surface-activated before the metal layer formation step. The surface activation treatment may be performed only on at least a portion of the metal layer, or only on at least a portion of the resin composition layer after exposure, or may be performed on at least a portion of both the metal layer and the resin composition layer after exposure. The surface activation treatment is preferably performed on at least a portion of the metal layer, and it is preferable to perform the surface activation treatment on part or all of the region of the metal layer on which the resin composition layer is to be formed. In this way, by performing the surface activation treatment on the surface of the metal layer, adhesion with the resin composition layer (film) provided on the surface can be improved. The surface activation treatment is also preferably performed on part or all of the resin composition layer (resin layer) after exposure. In this way, by performing the surface activation treatment on the surface of the resin composition layer, adhesion with the metal layer or resin layer provided on the surface that has been surface-activated can be improved. In particular, when negative development is performed, when the resin composition layer is cured, it is less susceptible to damage due to surface treatment and adhesion is likely to be improved. The surface activation treatment can be carried out, for example, by the method described in paragraph 0415 of International Publication No. 2021 / 112189. The contents of this specification are incorporated herein by reference.
[0412] <Semiconductor device and manufacturing method thereof> The present invention also discloses a semiconductor device including the cured product or laminate of the present invention. The present invention also discloses a manufacturing method of a semiconductor device including the manufacturing method of the cured product or the manufacturing method of the laminate of the present invention. Specific examples of semiconductor devices using the resin composition of the present invention to form an interlayer insulating film for a rewiring layer can be found in paragraphs 0213 to 0218 and FIG. 1 of JP 2016-027357 A, the contents of which are incorporated herein by reference.
[0413] <Photosensitizer> The present invention also relates to a photosensitizer represented by the following formula (z1).
[0414]
[0415] In formula (z1), R 9 ~R 12 each independently represents a monovalent organic group or a hydrogen atom. 2 represents a single bond or a divalent linking group. 11 and R 12 may be bonded to each other to form a ring.
[0416] R in formula (z1) 9 ~R 12 , and Z 2 The explanation, specific examples and preferred ranges of R in the above formula (b2) are 9 ~R 12 , and Z 2 is the same as
[0417] The present invention will be explained in more detail below with reference to examples. The materials, amounts used, ratios, processing details, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. Unless otherwise specified, "parts" and "%" are based on mass.
[0418] Examples and Comparative Examples In each example and comparative example, the components listed in Tables 1 to 9 below were mixed to obtain a resin composition. Specifically, the content of each component other than the solvent listed in Tables 1 to 9 was the amount (parts by mass) listed in the "Parts by Mass" column in each table. The amount of solvent used was adjusted to achieve the solid content concentration listed in the "Solid Content Concentration (% by Mass)" column in each table. The "mass ratio" of Solvent 1 and Solvent 2 is the content (% by mass) of each type of solvent relative to the total solvent. In each table, "-" indicates that the resin composition did not contain the corresponding component. The obtained resin composition was pressure-filtered using a polytetrafluoroethylene filter with a pore width of 0.5 μm.
[0419] Details of each component listed in each table are as follows:
[0420] [Resin] Resins A-1 to A-8 were used. The structural formula, weight average molecular weight (Mw), and molecular weight dispersity (Mw / Mn) of each resin are shown below. Mn is the number average molecular weight. The Mw and Mn of A-1 to A-8 were measured by the following method, not by the method described above. The Mw and Mn of A-1 to A-8 were values measured using gel permeation chromatography (GPC) and are polystyrene equivalent values. An HLC-8220GPC (manufactured by Tosoh Corporation) was used, and guard columns HZ-L, TSKgel Super HZM-M, TSKgel Super HZ4000, TSKgel Super HZ3000, and TSKgel Super HZ2000 (all manufactured by Tosoh Corporation) were connected in series. NMP was used as the eluent. A UV (ultraviolet) ray detector with a wavelength of 254 nm was used.
[0421]
[0422]
[0423] [Additive 1] A compound containing an anion shown in the "Anion species" column of each table and a cation shown in the "Cation species" column was used as Additive 1. The structural formulae of the anion and cation are shown below.
[0424]
[0425]
[0426]
[0427]
[0428] [Additive 2] The structural formula of the compound used as Additive 2 is shown below.
[0429]
[0430] [Additive Polymer] The following additive polymers were used: J-1: X-52-854 (silicone resin powder) manufactured by Shin-Etsu Silicone Co., Ltd. J-2: Zylon (modified polyphenylene ether / polystyrene polymer alloy) manufactured by Asahi Kasei Corporation J-3: FD PEEK 770PF (polyether ether ketone resin) manufactured by Jilin Joinature Polymer
[0431] The structural formulae of the compounds used as the silane coupling agent, migration inhibitor, and crosslinking agent are shown below.
[0432]
[0433] [Solvent] DMSO: dimethyl sulfoxide GBL: γ-butyrolactone
[0434] A synthesis example of the compound used as additive 1 (a photosensitizer containing cation C-9 and anion B-1) is shown below. Compounds containing C-3, C-4, C-5, C-6, C-8, C-10, C-14, or C-15 instead of C-9 as the cation can also be synthesized in the same manner. Compounds containing an anion other than B-1 as the anion can also be synthesized in the same manner. 10.0 g (39.33 mmol) of ketoprofen and 6.45 g (39.33 mmol) of 4-(chloromethyl)pyridine hydrochloride were dissolved in 130 ml of N-methyl-2-pyrrolidone (NMP), and 9.18 g (90.72 mmol) of triethylamine was added and stirred at 95°C for 2 hours. The solution was diluted with saturated NaHCO 3An aqueous solution was added, and the mixture was extracted with ethyl acetate. The organic layer was then washed with water. Magnesium sulfate was added to the resulting organic layer, stirred, and then filtered to remove the magnesium sulfate. The solvent was evaporated to dryness using a rotary evaporator to obtain a pyridine derivative. 30.0 g of methyl tosylate and 20.0 g of acetone were added to 15.0 g of the resulting pyridine derivative and stirred at room temperature (23°C) for 5 hours. After dilution with 50.0 g of acetone, the mixture was added dropwise to a hexane / ethyl acetate solution (1000 ml / 100 ml) to cause precipitation. The supernatant was removed, and 500 ml of hexane was added to the resulting solid. After stirring for 15 minutes, the supernatant was removed and the mixture was air-dried to obtain the tosylate salt. 20.0 g of the resulting tosylate salt was dissolved in 100 ml of methanol, and 10.0 g of sodium tetraphenylborate was added portionwise while stirring, resulting in precipitation of a solid. The resulting solid was filtered, washed with methanol, and air-dried to obtain the desired borate salt.
[0435] A synthesis example of the compound used as additive 1 (a photosensitizer containing cation C-1 and anion B-1) is shown below. Compounds containing C-7 instead of C-1 as the cation can also be synthesized in the same manner. Compounds containing anions other than B-1 as the anion can also be synthesized in the same manner. A solution of 15.0 g (91.45 mmol) of 3-(chloromethyl)pyridine hydrochloride in 200 ml of tetrahydrofuran (THF) was cooled to 0°C, and then 95.0 ml of tert-butylmagnesium chloride (23% by mass THF solution, approximately 2 mol / L) was slowly added dropwise and stirred for 1 hour. Water was added to the solution, and the mixture was extracted with ethyl acetate. Magnesium sulfate was added to the resulting organic layer, and after stirring, the magnesium sulfate was removed by filtration. The solvent was evaporated to dryness using a rotary evaporator to obtain a pyridine derivative. The target product was obtained by the same procedures as above.
[0436] A synthesis example of the compound used as additive 1 (a photosensitizer containing cation C-2 and anion B-1) is shown below. Compounds containing anions other than B-1 can also be synthesized in a similar manner. 8.00 g (61.43 mmol) of 1-nonanol was dissolved in 150 ml of N,N-dimethylformamide (DMF), and 6.00 g of NaH (60% by mass in oil) was added and stirred for 10 minutes. Next, 10.1 g (61.60 mmol) of 4-(chloromethyl)pyridine hydrochloride was slowly added, followed by stirring for an additional hour. Methanol was added until no more bubbles were generated, followed by addition of hexane. After stirring, the hexane layer was removed. Water was added to the remaining organic layer, and the mixture was extracted with ethyl acetate. Magnesium sulfate was added to the resulting organic layer, and after stirring, the magnesium sulfate was removed by filtration. The solvent was evaporated to dryness using a rotary evaporator, yielding a pyridine derivative. The target product was obtained by the same procedure as above.
[0437] A synthesis example of the compound used as additive 1 (a photosensitizer containing cation C-11 and anion B-1) is shown below. Compounds containing C-12 or C-18 as the cation instead of C-11 can also be synthesized in the same way. Compounds containing an anion other than B-1 as the anion can also be synthesized in the same way. 5.00 g (36.71 mmol) of 4-(ethylaminomethyl)pyridine was dissolved in 100 ml of NMP, and 9.50 g (36.71 mmol) of 9-fluorenylmethyl chloroformate was added and stirred for 2 hours. The solution was diluted with saturated NaHCO 3 An aqueous solution was added, and the mixture was extracted with ethyl acetate, followed by washing the organic layer with water. Magnesium sulfate was added to the resulting organic layer, and after stirring, the magnesium sulfate was removed by filtration. The solvent was evaporated to dryness using a rotary evaporator to obtain the pyridine derivative. The target product was obtained by the same procedure as above.
[0438] A synthesis example of the compound used as additive 1 (a photosensitizer containing cation C-13 and anion B-1) is shown below. Compounds containing anions other than B-1 can be synthesized in the same manner. 100 ml of THF was added to 5.00 g (36.71 mmol) of 4-(ethylaminomethyl)pyridine, and 9.59 g (50.00 mmol) of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride was added. 6.03 g (36.71 mmol) of o-coumaric acid was then slowly added, followed by stirring for 18 hours. Water was added to the solution, and the mixture was extracted with ethyl acetate. The resulting organic layer was washed twice with water, and then magnesium sulfate was added to the organic layer. After stirring, the magnesium sulfate was removed by filtration, and the solvent was evaporated to dryness using a rotary evaporator, yielding a pyridine derivative. The target product was obtained in the same manner as above, except that tosylic acid was used instead of methyl tosylate.
[0439] A synthesis example of the compound used as additive 1 (a photosensitizer containing cation C-20 and anion B-1) is shown below. Compounds containing C-16, C-17, or C-19 as the cation instead of C-20 can also be synthesized in the same manner. Compounds containing anions other than B-1 as the anion can also be synthesized in the same manner. 7.50 g (45.72 mmol) of 4-(chloromethyl)pyridine hydrochloride was dissolved in 120 ml of DMF, and 4.00 g of NaH (60% in oil) was added and stirred for 10 minutes. Next, 12.3 g (45.72 mmol) of 4-bromomethyl-7-methoxycoumarin (Br-Mmc) was slowly added, followed by stirring for an additional hour. Methanol was added until no more bubbles were generated, followed by addition of hexane. After stirring, the hexane layer was removed. Water was added to the remaining organic layer, followed by extraction with ethyl acetate. Magnesium sulfate was added to the obtained organic layer, and after stirring, the magnesium sulfate was removed by filtration, and the solvent was evaporated to dryness using a rotary evaporator to obtain a pyridine derivative.
[0440] A synthesis example of the compound used as additive 1 (a photosensitizer containing a cation CR-1 and an anion B-1) is shown below. Compounds containing anions other than B-1 can be synthesized in a similar manner. 6.00 g (26.47 mmol) of 9-chloromethylanthracene and 4.03 g (26.47 mmol) of DBU were dissolved in 70 ml of toluene and stirred at 95°C for 2 hours. The solution was filtered to obtain a quaternary ammonium salt. This quaternary ammonium salt was then dissolved in 100 ml of methanol, and 10.0 g of sodium tetraphenylborate was added little by little with stirring, resulting in the precipitation of a solid. The resulting solid was filtered, washed with methanol, and air-dried to obtain the desired borate salt.
[0441] <Preparation of Cured Film> In each Example and Comparative Example, a resin composition was applied to a silicon wafer by spin coating to form a coating film. The silicon wafer with the coating film was dried on a hot plate at 100°C for 5 minutes, yielding a uniform film (unexposed film) with a thickness of 15 μm on the silicon wafer. A photomask was attached to the unexposed film, and the unexposed film was pattern-exposed to light with a wavelength of 365 nm at a predetermined exposure dose (the exposure energy at a wavelength of 365 nm required to produce a good rectangular structure), forming exposed and unexposed areas. In Examples 30 to 32, the exposed film was heated on a hot plate for 5 minutes at the temperature listed in the table. The exposed film was then sprayed with the developer listed in each table, followed by spraying with water as the rinse solution when water or a 0.29% by weight aqueous solution of tetramethylammonium hydroxide (TMAH) was used as the developer, or PGMEA as the rinse solution when used otherwise, to obtain a pattern. Finally, the film was oven-heated at 350°C for 3 hours to obtain a cured film. The developer used is listed in the "Developer" column of each table. Also, the "Image Formation" column of each table indicates whether the development was negative or positive. S-1 and S-2 used as developers were cyclopentanone and a 0.29% by mass aqueous solution of tetramethylammonium hydroxide (TMAH), respectively.
[0442] <Evaluation> [Dielectric loss tangent] The silicon wafer having the cured film prepared above was immersed in a 3 mass % hydrofluoric acid aqueous solution to peel the cured film from the silicon wafer. The film thickness of the peeled cured film was 10 to 15 μm. The dielectric loss tangent of the peeled cured film at 28 GHz was measured using a resonator.
[0443] [Resolution] As described above, the developer shown in each table was sprayed onto the exposed film, and a rinse solution was sprayed onto the film as described above to obtain a pattern. The pattern of the obtained cured film was observed, and the line width that had good edge sharpness was evaluated according to the following criteria. The smaller the line width, the greater the difference in solubility in the developer between the exposed and unexposed areas, and the better the resolution. Evaluation was based on the following criteria. 4: Line width is 1 μm or less 3: Line width is more than 1 μm and less than 5 μm 2: Line width is more than 5 μm and less than 10 μm 1: Line width is more than 10 μm
[0444] [Low-Temperature Curing] When a polyimide precursor is used as the resin, the film developed in the above <Preparation of Cured Film> is heat-treated at a certain temperature for 3 hours, and the infrared absorption spectrum is measured. The absorption peak at 1377 cm -1 Next, the peak intensity P1 around 1490 cm -1 The infrared absorption spectrum was measured again after heat treatment of the film at 350 °C for 3 hours. -1 The peak intensity P2 around 1490 cm -1 The absorption intensity of the aromatic rings observed near the peak intensity P1 is normalized. Using the normalized values of the obtained peak intensities P1 and P2, the cyclization rate of the film can be calculated based on the following formula: Cyclization rate (%) = (normalized value of peak intensity P1) / (normalized value of peak intensity P2) × 100. Here, the temperature (°C) at which the cyclization rate reached 95% when the peak intensity P1 was calculated was measured.
[0445] When a polybenzoxazole precursor is used as the resin, the film developed in the above <Preparation of Cured Film> is heat-treated at a certain temperature for 3 hours, and the infrared absorption spectrum is measured. -1Next, the peak intensity Q1 around 1490 cm -1 Next, the film was heat-treated at 350°C for 3 hours, and the infrared absorption spectrum was measured again. -1 The peak intensity Q2 around 1490 cm -1 The peak intensity Q1 is normalized by the absorption intensity of the aromatic ring found near the peak Q1. Using the normalized values of the obtained peak intensities Q1 and Q2, the cyclization rate of the film can be calculated based on the following formula: Cyclization rate (%) = (normalized value of peak intensity Q1 / normalized value of peak intensity Q2) x 100. Here, the temperature (°C) at which the peak intensity Q1 was calculated and the cyclization rate reached 95% was measured.
[0446] When a polyimide precursor and a polybenzoxazole precursor are used in combination as the resin, the cyclization rate is calculated by the following formula: cyclization rate of polyimide precursor × weight of polyimide precursor / (weight of polyimide precursor + weight of polybenzoxazole precursor) + cyclization rate of polybenzoxazole × weight of polybenzoxazole precursor / (weight of polyimide precursor + weight of polybenzoxazole precursor). Here, the temperature (°C) at which the peak intensity P1 and peak intensity Q1 were found and the value of the above formula was 95% was measured.
[0447] When polyimide or polybenzoxazole is used as the resin, this is the minimum temperature required to achieve the desired resolution and dielectric loss tangent. Specifically, this is the minimum temperature (°C) required to achieve a resolution of 4 or 3 according to the above evaluation criteria and a dielectric loss tangent of 0.008 or less according to the above evaluation method.
[0448] [Sensitivity] The exposure energy at a wavelength of 365 nm required to form a good rectangular structure using the above-mentioned predetermined exposure dose was evaluated as follows. The lower the exposure energy, the higher the sensitivity and the better the results. Evaluation was based on the following criteria: 4: Exposure energy is 100 mJ or less 3: Exposure energy is more than 100 mJ and less than 400 mJ 2: Exposure energy is more than 400 mJ and less than 1000 mJ 1: Exposure energy is more than 1000 mJ
[0449] The evaluation results for each of the Examples and Comparative Examples are shown in the following Tables 1 to 9. In the tables, the unit for "low temperature curing" is "°C."
[0450]
[0451]
[0452]
[0453]
[0454]
[0455]
[0456]
[0457]
[0458]
[0459] From the above results, it is clear that the cured film made of the resin composition of the present invention has a low dielectric loss tangent. It is also clear that the resin composition of the present invention has excellent resolution. Furthermore, it is clear that the resin composition of the present invention has excellent curing properties at low temperatures and excellent sensitivity.
[0460] Example 101 The resin composition used in Example 5 was applied by spin coating to the surface of the thin copper layer of a resin substrate having a thin copper layer formed on its surface. The resulting film was dried at 100°C for 4 minutes to form a 20 μm-thick film, which was then exposed using a stepper (Nikon Corporation, NSR1505 i6). The exposure was performed at a wavelength of 365 nm through a mask (a binary mask with a 1:1 line-and-space pattern and a line width of 10 μm). After exposure, the film was heated at 100°C for 4 minutes. After the heating, the film was developed with cyclohexanone for 2 minutes and rinsed with PGMEA for 30 seconds to obtain a layer pattern. The temperature was then increased at a rate of 10°C / min in a nitrogen atmosphere, reaching 230°C, and maintained at 230°C for 3 hours to form an interlayer insulating film for a redistribution layer. This interlayer insulating film for a redistribution layer had excellent insulating properties. Furthermore, semiconductor devices were manufactured using these interlayer insulating films for a redistribution layer, and it was confirmed that they operated without any problems.
[0461] According to the present invention, it is possible to provide a resin composition that can obtain a film with a low dielectric tangent and has excellent resolution, a method for producing an interlayer insulating film for a redistribution layer using the resin composition, and a photosensitizer that can be used in the resin composition.
[0462] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2023-054395) filed on March 29, 2023, the contents of which are incorporated herein by reference.
Claims
1. A resin composition comprising an anion represented by the following formula (a1), a cation represented by the following formula (b1), and a resin: In formula (a1), R 1 ~R 3 R each independently represents a hydrogen atom, a halogen atom, a hydroxyl group, an alkyl group, an alkenyl group, an alkynyl group, or an aryl group. 4 ~R 8 R each independently represents a halogen atom, a monovalent organic group, or a hydrogen atom. 4 ~R 8 In formula (b1), at least two of R may be bonded to form a ring. 9 ~R 12 R each independently represents a monovalent organic group or a hydrogen atom. 13 represents a monovalent organic group. 2 represents a single bond or a divalent linking group. p represents an integer of 1 to 5. q represents an integer of 0 to 4. R 10 When there are multiple R 10 may be the same or different. 11 and R 12 may be bonded to each other to form a ring. 11 When there are multiple R 11 may be the same or different, and at least two of them may be bonded to each other to form a ring. 12 When there are multiple R 12 may be the same or different, and at least two of them may be bonded to each other to form a ring. 13 When there are multiple R 13 may be the same or different, and at least two of them may be bonded to each other to form a ring.
2. The resin composition according to claim 1, wherein the anion is represented by the following formula (a2): In formula (a2), a to d each independently represent an integer of 0 to 5. 21 ~R 24 R each independently represents a halogen atom or a monovalent organic group. 21 When there are multiple R 21 may be the same or different, and at least two of them may be bonded to each other to form a ring. 22 When there are multiple R 22 may be the same or different, and at least two of them may be bonded to each other to form a ring. 23 When there are multiple R 23 may be the same or different, and at least two of them may be bonded to each other to form a ring. 24 When there are multiple R 24 may be the same or different, and at least two of them may be bonded to each other to form a ring.
3. The resin composition according to claim 1, wherein the anion is represented by the following formula (a3):
4. The resin composition according to claim 1, wherein the cation is represented by the following formula (b2): In formula (b2), R 9 ~R 12 each independently represents a monovalent organic group or a hydrogen atom. 2 R represents a single bond or a divalent linking group. 11 and R 12 may be bonded to each other to form a ring.
5. Z in the formula (b1) 2 is a single bond, -O-, -S-, -NR 14 -, *-OC(=O)-#, *-SC(=O)-#, *-NR 15 C(=O)-#, -OC(=O)O-, *-OC(=O)S-#, *-SC(=O)O-#, -SC(=O)S-, *-NR 16 C(=O)O-#, *-OC(=O)NR 17 -#, *-NR 18 C(=O)NR 19 -# or *-OS (=O) 2 - #, R 14 ~R 19 each independently represents a hydrogen atom, an alkyl group, or an aryl group, and * represents R 11 and R 12 represents the bond position with the carbon atom to which it is bonded, and # represents R 10 The resin composition according to claim 1 , wherein the bond site is 6. The resin composition according to claim 1, wherein the resin comprises at least one selected from the group consisting of polyimide, polyimide precursor, polybenzoxazole and polybenzoxazole precursor.
7. The resin composition according to claim 1, which is used for organic solvent development.
8. The resin composition according to claim 1, which is used in aqueous solution development.
9. The resin composition according to claim 1, which is used to form an interlayer insulating film for a rewiring layer.
10. A method for manufacturing an interlayer insulating film for a redistribution layer, comprising: a photosensitive film forming step of applying the resin composition according to any one of claims 1 to 9 onto a substrate to form a photosensitive film; an exposure step of exposing the photosensitive film to light to form an exposed film; and a pattern forming step of developing the exposed film with a developer to form an insulating pattern.
11. The method for producing an interlayer insulating film for a rewiring layer according to claim 10, wherein the developer is an organic solvent.
12. The method for producing an interlayer insulating film for a rewiring layer according to claim 10, wherein the developer is an aqueous solution.
13. A photosensitizer represented by the following formula (z1): In formula (z1), R 9 ~R 12 each independently represents a monovalent organic group or a hydrogen atom. 2 R represents a single bond or a divalent linking group. 11 and R 12 may be bonded to each other to form a ring.
Citation Information
Patent Citations
Cyanine-based organic coloring metter, photopolymerizable composition and recording material
JP2001226417A
Lithographic printing original plate
JP2013205519A