Pressure-sensitive adhesive, method for producing pressure-sensitive adhesive, and pressure-sensitive adhesive sheet

The polyester pressure-sensitive adhesive with controlled molecular weight and silicone surfactant addresses environmental concerns and coating defects, offering enhanced performance and sustainability by using biopolyester resin and minimizing solvent use.

WO2024203232A1PCT designated stage expired Publication Date: 2024-10-03NITTO DENKO CORP

Patent Information

Application Number
PCT/JP2024/009357
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-11
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional pressure-sensitive adhesives face challenges in reducing environmental impact while maintaining excellent coating properties, particularly when using low molecular weight polyester resins that require minimal organic solvents, as they can lead to deteriorated workability and coating defects.

Method used

A polyester pressure-sensitive adhesive is developed with a weight average molecular weight of 0.2×10^4 to 2.0×10^4, incorporating a surfactant to adjust viscosity and surface tension, specifically using a silicone surfactant to prevent coating defects, and utilizing a biopolyester resin to minimize environmental impact without organic solvents.

Benefits of technology

The solution provides a pressure-sensitive adhesive with improved coating properties and reduced environmental impact by maintaining adhesive strength and preventing coating defects, while minimizing solvent use and promoting sustainable practices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009357_03102024_PF_FP_ABST
    Figure JP2024009357_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a polyester-based pressure-sensitive adhesive that can contribute to reducing environmental impact, wherein the polyester-based pressure-sensitive adhesive has excellent coating properties. A polyester-based pressure-sensitive adhesive according to one embodiment of the present invention contains a polyester-based resin and a surfactant. The weight-average molecular weight of the polyester-based resin is 0.2×104 to 2.0×104, and the viscosity of the polyester-based pressure-sensitive adhesive is 1-50 Pa∙s. The polyester-based pressure-sensitive adhesive may be substantially free of organic solvents.
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive, method for producing adhesive, and adhesive sheet

[0001] The present invention relates to a pressure-sensitive adhesive, a method for producing a pressure-sensitive adhesive, and a pressure-sensitive adhesive sheet.

[0002] Pressure-sensitive adhesives have been used in various technical fields. In addition to acrylic pressure-sensitive adhesives, polyester pressure-sensitive adhesives have also been considered for use as pressure-sensitive adhesives from the viewpoint of optimizing adhesive strength.

[0003] On the other hand, the demand for reducing environmental impact is increasing year by year, and pressure sensitive adhesives are also being required to reduce environmental impact during production, use, etc.

[0004] JP 2020-056006 A JP 2003-238930 A

[0005] One way to reduce the environmental load is to reduce the amount of solvent used. However, when preparing a PSA with a low solvent content, it may be necessary to reduce the molecular weight of the base polymer (e.g., polyester resin) in the PSA, and the low molecular weight of the base polymer may cause deterioration in coatability.

[0006] The present invention has been made to solve the above-mentioned conventional problems, and an object of the present invention is to provide a polyester-based pressure-sensitive adhesive that can contribute to reducing the environmental load and has excellent coatability.

[0007] [1] A polyester-based pressure-sensitive adhesive according to one embodiment of the present invention comprises a polyester-based resin and a surfactant, and the weight-average molecular weight of the polyester-based resin is 0.2 × 10 4 ~2.0 x 10 4and the viscosity of the polyester-based pressure-sensitive adhesive is 1 Pa·s to 50 Pa·s. [2] The polyester-based pressure-sensitive adhesive according to [1] above may be substantially free of organic solvents. [3] In the polyester-based pressure-sensitive adhesive according to [1] or [2] above, the surface tension of the polyester-based pressure-sensitive adhesive may be 30 mN / m or less. [4] In the polyester-based pressure-sensitive adhesive according to any one of [1] to [3] above, the polyester-based resin may be a biopolyester-based resin. [5] In the polyester-based pressure-sensitive adhesive according to any one of [1] to [4] above, the surfactant may be a silicone-based surfactant. [6] A method for producing a polyester-based pressure-sensitive adhesive according to one embodiment of the present invention comprises mixing a polyester-based resin and a surfactant to prepare a mixture, the mixture being substantially free of organic solvents. [7] A pressure-sensitive adhesive sheet according to one embodiment of the present invention comprises a pressure-sensitive adhesive layer comprising the polyester-based pressure-sensitive adhesive according to any one of [1] to [5] above. [8] The pressure-sensitive adhesive sheet according to the above item [7] may have an adhesive strength of 5 N / 20 mm or more at 23° C. when the pressure-sensitive adhesive layer is attached to an SUS304 plate. [9] The pressure-sensitive adhesive sheet according to the above item [7] or [8] may have a haze value of 0.1% to 5%.

[0008] According to the present invention, it is possible to provide a polyester-based pressure-sensitive adhesive that can contribute to reducing the environmental load and has excellent coatability.

[0009] 1( a ) and 1 ( b ) are schematic cross-sectional views of a pressure-sensitive adhesive sheet according to one embodiment of the present invention.

[0010] A. Polyester-Based Pressure-Sensitive Adhesive The polyester-based pressure-sensitive adhesive according to an embodiment of the present invention has a weight-average molecular weight of 0.2×10 4 ~2.0 x 10 4 The polyester-based adhesive contains a polyester resin having a viscosity of 1 Pa·s to 50 Pa·s.

[0011] In an embodiment of the present invention, by adding a surfactant and adjusting the viscosity to the above range, the surface tension of the PSA can be preferably adjusted, and as a result, a polyester-based PSA having excellent coatability can be provided even when a low-molecular-weight polyester-based resin is used. By using a low-molecular-weight polyester-based resin, the amount of organic solvent added can be reduced, resulting in a polyester-based PSA with a low environmental impact.

[0012] Preferably, the polyester-based PSA is substantially free of organic solvents. By being substantially free of organic solvents, a polyester-based PSA with low environmental impact can be provided. The concept of "substantially free of organic solvents" (hereinafter also referred to as "solvent-free") can also include embodiments in which a small amount of organic solvent inevitably present in raw materials or unintentionally mixed in during production is contained. However, the amount of unintentionally contained organic solvent is preferably 3 parts by weight or less, more preferably 1 part by weight or less, more preferably 0.5 parts by weight or less, and particularly preferably 0.1 parts by weight or less per 100 parts by weight of the polyester-based PSA.

[0013] As described above, the viscosity of the polyester-based pressure-sensitive adhesive at 25°C is 1 Pa·s to 50 Pa·s, more preferably 2 Pa·s to 40 Pa·s, and even more preferably 2.5 Pa·s to 20 Pa·s. Within this range, a polyester-based pressure-sensitive adhesive with significantly excellent coatability can be obtained. In this specification, viscosity refers to a viscosity at 0.1 to 1000 (1 / s) measured using a rheometer.

[0014] The surface tension of the polyester-based PSA is preferably 50 mN / m or less, more preferably 30 mN / m or less, and even more preferably 10 mN / m to 25 mN / m. Within this range, a polyester-based PSA capable of forming a PSA layer without coating defects can be obtained. In one embodiment, the surface tension of the polyester-based PSA is 5 mN / m to 28 mN / m (preferably 10 mN / m to 25 mN / m). By using a silicone surfactant as the surfactant and adjusting the surface tension within the above range, a polyester-based PSA having a significant effect of preventing coating defects (e.g., cissing) can be obtained. Furthermore, when the viscosity of a polyester-based PSA at 25°C is 1 Pa·s to 20 Pa·s, adjusting the surface tension of the polyester-based PSA to 5 mN / m to 28 mN / m (preferably 10 mN / m to 25 mN / m) can be adjusted to 5 mN / m to 28 mN / m (preferably 10 mN / m to 25 mN / m) can be adjusted to a value that significantly prevents coating defects (e.g., cissing). The surface tension of the polyester-based pressure-sensitive adhesive can be measured by the pendant drop method.

[0015] The contact angle of the polyester-based PSA on polyethylene terephthalate is preferably 50° or less, more preferably 40° or less, and even more preferably 10° to 40°. Within this range, a polyester-based PSA capable of forming a PSA layer without coating defects can be obtained. In one embodiment, the contact angle of the polyester-based PSA on polyethylene terephthalate is 10° to 45° (preferably 15° to 40°). By using a silicone surfactant as the surfactant and adjusting the contact angle within the above range, a polyester-based PSA having a significant effect of preventing coating defects (e.g., cissing) can be obtained. Furthermore, when the viscosity of the polyester-based PSA at 25°C is 1 Pa·s to 50 Pa·s (preferably 2.5 Pa·s to 20 Pa·s), adjusting the contact angle to 10° to 45° (preferably 15° to 40°) can be obtained, which can significantly prevent coating defects (e.g., cissing).

[0016] (Polyester Resin) Typically, polyester resins are obtained by reacting a polycarboxylic acid component with a polyhydric alcohol component. The polycarboxylic acid component contains one or more compounds selected from polycarboxylic acids having two or more carboxyl groups in one molecule and their derivatives. The polyhydric alcohol component contains one or more compounds selected from polyhydric alcohols having two or more hydroxyl groups in one molecule.

[0017] In one embodiment, the polyester resin is a biopolyester resin. In this specification, the biopolyester resin refers to a polyester resin in which at least one of a polycarboxylic acid component and a polyhydric alcohol component is derived from a plant. By using the renewable plant-derived material, it is possible to obtain a polyester pressure-sensitive adhesive that can address the depletion of fossil resources and global warming and contribute to reducing the environmental impact.

[0018] Examples of the polycarboxylic acid include aliphatic or alicyclic dibasic acids. Specific examples include adipic acid, azelaic acid, dimer acid, sebacic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 4-methyl-1,2-cyclohexanedicarboxylic acid, dodecenylsuccinic anhydride, fumaric acid, succinic acid, dodecanedioic acid, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, maleic acid, maleic anhydride, itaconic acid, and citraconic acid. Aromatic dibasic acids may also be used. Specific examples of aromatic dibasic acids include terephthalic acid, isophthalic acid, orthophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 2,2'-diphenyldicarboxylic acid, and 4,4'-diphenyletherdicarboxylic acid. As the polycarboxylic acid derivative, anhydrides and alkyl esters (for example, monoesters, diesters, etc., preferably monoalcohols having 1 to 3 carbon atoms) of the above carboxylic acids can be used.

[0019] In one embodiment, a plant-derived polycarboxylic acid is used. Examples of plant-derived polycarboxylic acids include dimer acid, sebacic acid, succinic acid, and glutaric acid. Here, "dimer acid" refers to a dicarboxylic acid having a structure in which an unsaturated fatty acid is dimerized. A typical example of the dimer acid is a dicarboxylic acid having 36 carbon atoms and a structure in which an unsaturated fatty acid having 18 carbon atoms (oleic acid, linoleic acid, linolenic acid, etc.) is dimerized.

[0020] When the polycarboxylic acid component contains a plant-derived polycarboxylic acid, the content of the plant-derived polycarboxylic acid is preferably 10 mol % or more, preferably 50 mol % or more, more preferably 75 mol % or more, even more preferably 90 mol % or more, and most preferably 100 mol % based on the total amount of polycarboxylic acids in the polycarboxylic acid component.

[0021] Examples of the polyhydric alcohol include aliphatic or alicyclic diols, such as ethylene glycol, 1,2-propylene glycol, 1,3-propanediol, 2-methyl-1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, diethylene glycol, dipropylene glycol, 2,2,4-trimethyl-1,5-pentanediol, 2-ethyl-2-butylpropanediol, 1,9-nonanediol, 2-methyloctanediol, and 1,10-decanediol.

[0022] In one embodiment, a plant-derived polyhydric alcohol is used. Examples of plant-derived polyhydric alcohols include dimer diol, 1,3-propanediol, 1,4-butanediol, ethylene glycol, and polyoxytetramethylene glycol. Here, "dimer diol" refers to a diol having a structure in which the carboxyl group in a dicarboxylic acid formed by dimerization of an unsaturated fatty acid is converted to a hydroxyl group (hydrogenated). A diol having 36 carbon atoms corresponding to a dimer of an unsaturated fatty acid having 18 carbon atoms (oleic acid, linoleic acid, linolenic acid, etc.) is a typical example included in the above dimer diol.

[0023] When the polyhydric alcohol component contains a plant-derived polyhydric alcohol, the content of the plant-derived polyhydric alcohol is preferably 50 mol% or more, more preferably 75 mol% or more, even more preferably 90 mol% or more, and most preferably 100 mol% relative to the total polyhydric alcohols in the polyhydric alcohol component.

[0024] The polyester resin can be obtained by polycondensation of a polycarboxylic acid component and a polyhydric alcohol component. More specifically, the polyester resin can be produced (synthesized) by proceeding with the condensation reaction between a carboxyl group of the polycarboxylic acid component and a hydroxyl group of the polyhydric alcohol component, for example, while removing water (condensed water) produced by the condensation reaction from the reaction system. Methods for removing the condensed water from the reaction system include a method of blowing an inert gas into the reaction system and removing the condensed water together with the inert gas from the reaction system, and a method of distilling off the condensed water from the reaction system under reduced pressure (reduced pressure method). The reduced pressure method is preferably used because it is suitable for shortening the polymerization time and improving productivity.

[0025] The reaction conditions, such as the reaction temperature when carrying out the condensation reaction and the degree of vacuum (pressure in the reaction system) when a reduced pressure method is adopted, can be any appropriate conditions. The reaction temperature is, for example, 180°C to 260°C, and preferably 200°C to 220°C. The degree of vacuum is, for example, 10 kPa or less, preferably 0.1 kPa to 10 kPa, and more preferably 0.1 kPa to 4 kPa.

[0026] Any appropriate polymerization catalyst may be used in the condensation reaction. Examples of the polymerization catalyst include titanium-based catalysts such as tetraisopropyl titanate and tetrabutyl titanate, antimony-based catalysts such as antimony trioxide, germanium-based catalysts such as germanium dioxide, and catalysts such as zinc acetate, manganese acetate, and dibutyltin oxide. These catalysts may be used alone or in combination of two or more. Among these, antimony trioxide, tetrabutyl titanate, germanium dioxide, and zinc acetate are preferably used.

[0027] The amount of the polymerization catalyst may be any appropriate amount, and is, for example, preferably 0.001 mol % to 5 mol %, more preferably 0.01 mol % to 3 mol %, and even more preferably 0.1 mol % to 2 mol %, based on the total amount of the polycarboxylic acid component and the polyhydric alcohol component.

[0028] In one embodiment, the synthesis of the polyester resin can be carried out without using an organic solvent.

[0029] The content of the polyester resin is preferably 60 parts by weight or more, more preferably 70 parts by weight or more, and even more preferably 80 parts by weight or more, based on 100 parts by weight of the polyester pressure-sensitive adhesive.

[0030] As described above, the weight average molecular weight of the polyester resin is 0.2 × 10 4 ~2.0 x 10 4Within this range, a polyester-based pressure-sensitive adhesive capable of exhibiting appropriate adhesive strength can be preferably prepared without the inclusion of a solvent. The present invention is advantageous in that excellent coating properties are achieved even when a polyester-based resin having such a low weight-average molecular weight is used. Details will be described later. The weight-average molecular weight of the polyester-based resin is preferably 0.25 × 10 4 ~1.5 x 10 4 and more preferably 0.3 × 10 4 ~1.0 x 10 4 Within this range, the above-mentioned effects become significant. In this specification, the weight average molecular weight refers to a value calculated in terms of polystyrene measured by gel permeation chromatography (GPC).

[0031] (Surfactant) As described above, the polyester-based PSA contains a surfactant. In an embodiment of the present invention, even when a polyester-based resin having a low molecular weight is used, by adding a surfactant, a polyester-based PSA having excellent coatability can be obtained. More specifically, when a low-molecular-weight polyester-based resin is used in a solvent-free preparation, coating defects such as repelling may occur when the PSA is applied to a substrate (such as a release liner). In the present invention, however, by adding a surfactant, such coating defects can be prevented.

[0032] Any suitable surfactant can be used as long as the effects of the present invention can be obtained. Preferably, a silicone surfactant is used as the surfactant. By controlling the surface tension of the polyester-based pressure-sensitive adhesive with a silicone surfactant, it is possible to obtain a polyester-based pressure-sensitive adhesive that can form a pressure-sensitive adhesive layer without coating defects. The silicone-based surfactant can be a compound containing a structural unit having a siloxane bond in the main chain, and can be a compound containing a hydrophobic part and a hydrophilic part in one molecule. The silicone-based surfactant is preferably a compound that does not contain a fluorine atom. The use of such a silicone-based surfactant makes the above-mentioned effects more pronounced.

[0033] In one embodiment, the silicone surfactant is preferably a modified silicone compound. Examples of the modified silicone compound include compounds having a structure in which an organic group is introduced into the side chain and / or terminal of a polysiloxane. Examples of the organic group include a group containing a functional group selected from an amino group, an epoxy group, an alicyclic epoxy group, a carbinol group, a mercapto group, a carboxyl group, a fatty acid ester group, and a fatty acid amide group, and a group containing a polyether chain.

[0034] In one embodiment, a polyether-modified silicone compound is used as the silicone surfactant. The use of a polyether-modified silicone compound significantly enhances the above-described effects. Examples of polyether-modified silicone compounds include polyether-modified polydimethylsiloxane and polyether-modified polymethylalkylsiloxanes in which one of the dimethyl groups of polydimethylsiloxane is partially or entirely substituted with a long-chain alkyl group. Specific examples of these include polydimethylsiloxanes modified with polyethylene oxide, polypropylene oxide, polybutylene oxide, or a mixture thereof. These polyether-modified polydimethylsiloxanes can be obtained by appropriately changing the amounts and mixing ratios of polyethylene oxide, polypropylene oxide, or polybutylene oxide.

[0035] As the polyether-modified silicone compound, commercially available products may be used, and examples thereof include BYK-333, BYK-378, BYK-3760, BYK-330, and BYK-329 manufactured by BYK Japan KK.

[0036] The content of the surfactant is preferably 0.1 to 15 parts by weight, more preferably 0.2 to 10 parts by weight, and even more preferably 0.3 to 8 parts by weight, relative to 100 parts by weight of the polyester resin. Within such a range, a polyester-based pressure-sensitive adhesive capable of forming a pressure-sensitive adhesive layer without coating defects can be obtained.

[0037] (Other Additives) The polyester-based pressure-sensitive adhesive may further contain any appropriate additives as necessary. Examples of additives include crosslinkers, inorganic particles, tackifiers, plasticizers (e.g., trimellitic ester-based plasticizers, pyromellitic ester-based plasticizers, etc.), pigments, dyes, fillers, antioxidants, conductive materials, antistatic agents, UV absorbers, light stabilizers, release adjusters, softeners, flame retardants, antioxidants, etc. The polyester-based pressure-sensitive adhesive may also further contain other resins such as acrylic resins, natural rubber resins, synthetic rubber resins, and silicone resins.

[0038] In one embodiment, the polyester-based pressure-sensitive adhesive contains a crosslinking agent. In one embodiment, an isocyanate-based crosslinking agent and / or an epoxy-based crosslinking agent is used as the crosslinking agent. In one embodiment, the content of the crosslinking agent is 3 parts by weight or more relative to 100 parts by weight of the polyester-based resin.

[0039] The isocyanate crosslinking agent is a compound having an isocyanate group, and specific examples thereof include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate; aromatic isocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate and xylylene diisocyanate; and isocyanate adducts such as trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., trade name "Coronate L"), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., trade name "Coronate HL"), and isocyanurate of hexamethylene diisocyanate (manufactured by Nippon Polyurethane Industry Co., Ltd., trade name "Coronate HX"). When the polyester-based pressure-sensitive adhesive contains an isocyanate-based crosslinking agent, the content of the isocyanate-based crosslinking agent can be set to any appropriate amount depending on the desired adhesive strength, and is preferably 3 to 30 parts by weight, more preferably 10 to 20 parts by weight, relative to 100 parts by weight of the polyester-based resin.

[0040] The epoxy crosslinking agent is a compound having an epoxy group, and specific examples thereof include N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, 1,3-bis(N,N-glycidylaminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Company, Inc., trade name "Tetrad C"), 1,6-hexanediol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 1600"), neopentyl glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 1500N"), and 1,6-hexanediol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 1500N"). P"), ethylene glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 40E"), propylene glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 70P"), polyethylene glycol diglycidyl ether (manufactured by NOF Corporation, trade name "Epiol E-400"), polypropylene glycol diglycidyl ether (manufactured by NOF Corporation, trade name "Epiol P-200"), sorbitol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol" EX-611), glycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol EX-314"), pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol EX-512"), sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. When the polyester-based pressure-sensitive adhesive contains an epoxy-based crosslinking agent, the content of the epoxy-based crosslinking agent can be set to any appropriate amount depending on the desired adhesive strength, and is typically 0.01 to 10 parts by weight, and more preferably 3 to 5 parts by weight, relative to 100 parts by weight of the polyester-based resin.

[0041] In one embodiment, the polyester-based pressure-sensitive adhesive contains a crosslinking catalyst. Examples of the crosslinking catalyst include metal complex compounds such as aluminum triacetylacetonate, iron triacetylacetonate, manganese tetraacetylacetonate, nickel tetraacetylacetonate, chromium hexaacetylacetonate, titanium tetraacetylacetonate, and cobalt tetraacetylacetonate; metal alkoxides such as aluminum ethoxide, aluminum propoxide, aluminum butoxide, titanium ethoxide, titanium propoxide, and titanium butoxide; metal salt compounds such as sodium acetate, tin octoate, lead octoate, cobalt octoate, zinc octoate, calcium octoate, lead naphthenate, cobalt naphthenate, dibutyltin dioctate, dibutyltin dilaurate, dibutyltin maleate, and dibutyltin di(2-ethylhexoate); formic acid, acetic acid, propionic acid, and p-toluenesulfonyl ether. acidic compounds such as toluenesulfonic acid, trichloroacetic acid, phosphoric acid, monoalkyl phosphoric acid, dialkyl phosphoric acid, phosphate ester of β-hydroxyethyl (meth)acrylate, monoalkyl phosphorous acid, dialkyl phosphorous acid; acids such as p-toluenesulfonic acid, phthalic anhydride, benzoic acid, benzenesulfonic acid, dodecylbenzenesulfonic acid, formic acid, acetic acid, itaconic acid, oxalic acid, maleic acid, and the like; and ammonium salts, lower amine salts, polyvalent metal salts thereof; organometallic compounds such as sodium hydroxide, lithium chloride, diethylzinc, and tetra(n-butoxy)titanium; and amines such as dicyclohexylamine, triethylamine, N,N-dimethylbenzylamine, N,N,N',N'-tetramethyl-1,3-butanediamine, diethanolamine, triethanolamine, and cyclohexylethylamine.

[0042] The content of the crosslinking catalyst is preferably 0.01 to 1 part by weight, more preferably 0.05 to 0.8 parts by weight, and even more preferably 0.08 to 0.5 parts by weight, relative to 100 parts by weight of the polyester resin. Within such a range, a polyester pressure-sensitive adhesive that prevents coating defects can be obtained.

[0043] In one embodiment, the polyester-based pressure-sensitive adhesive contains inorganic particles. The inorganic particles may be inorganic particles that can impart thixotropy to the polyester-based pressure-sensitive adhesive.

[0044] Examples of the inorganic particles include silica, titanium dioxide, bentonite, zinc oxide, talc, kaolin, mica, vermiculite, magnesium carbonate, calcium carbonate, aluminum silicate, barium silicate, calcium silicate, magnesium silicate, strontium silicate, metal tungstate, magnesium, zeolite, barium sulfate, calcined calcium sulfate, calcium phosphate, fluorapatite, hydroxyapatite, and metal soap. Composite particles obtained by coating particles with a metal oxide or the like, or modified particles whose particle surfaces have been treated with a compound or the like, may also be used. Among these, silica particles are preferably used, and fumed silica is more preferably used.

[0045] The content of the inorganic particles is preferably 1 to 30 parts by weight, more preferably 3 to 20 parts by weight, and even more preferably 3 to 10 parts by weight, relative to 100 parts by weight of the polyester resin. Within such a range, a polyester pressure-sensitive adhesive that prevents coating defects can be obtained.

[0046] B. Method for Producing a Polyester-Based Pressure-Sensitive Adhesive A method for producing a polyester-based pressure-sensitive adhesive according to an embodiment of the present invention includes mixing a polyester-based resin and a surfactant to prepare a mixture, and the mixture is characterized by being substantially free of organic solvents.

[0047] In one embodiment, the polyester-based resin used in the above production method is the polyester-based resin described in the above section A. However, in the above production method, the polyester-based resin has a weight-average molecular weight of 0.2 × 10 4 ~2.0 x 10 4 In place of such a polyester resin, a polyester resin having a molecular weight outside the above range may be used as long as the effects of the present invention can be obtained.

[0048] The surfactant used may be any of those described in Section A. The mixture may further contain an additive (e.g., a crosslinking agent) described in Section A.

[0049] The mixture may be prepared by any suitable method.

[0050] C. Pressure-Sensitive Adhesive Sheet In one embodiment, a pressure-sensitive adhesive sheet is provided, which includes a pressure-sensitive adhesive layer containing the polyester-based pressure-sensitive adhesive. Figure 1 is a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to one embodiment of the present invention. The pressure-sensitive adhesive sheet 100 may be composed of only a pressure-sensitive adhesive layer 10, as shown in Figure 1(a), or may be composed of a substrate 20 and a pressure-sensitive adhesive layer 10 disposed on at least one side of the substrate 20, as shown in Figure 1(b).

[0051] The thickness of the pressure-sensitive adhesive sheet is preferably 3 μm to 300 μm, more preferably 5 μm to 150 μm, and even more preferably 10 μm to 100 μm.

[0052] The adhesive strength at 23°C when the adhesive layer of the pressure-sensitive adhesive sheet is attached to a SUS304 plate is not particularly limited and can be adjusted to an appropriate range depending on the purpose and application. The adhesive strength may be, for example, 0.5 N / 20 mm or more, or 0.8 N / 20 mm or more. A pressure-sensitive adhesive sheet exhibiting an adhesive strength of a predetermined value or more can adhere well to an adherend. From this perspective, in some embodiments, the adhesive strength is preferably 1.0 N / 20 mm or more, more preferably 1.5 N / 20 mm or more, even more preferably 2.0 N / 20 mm or more, and may be 2.5 N / 20 mm or more, 3.0 N / 20 mm or more, 3.5 N / 20 mm or more, 4.0 N / 20 mm or more, 4.5 N / 20 mm or more, or 5 N / 20 mm or more. The upper limit of the adhesive strength is not particularly limited and may be, for example, less than 30 N / 20 mm, or may be 25 N / 20 mm or less, 20 N / 20 mm or less, or 15 N / 20 mm or less from the viewpoint of easily balancing with other properties, etc. The adhesive strength refers to the adhesive strength measured by a method in accordance with JIS Z 0237:2009 (lamination conditions: one reciprocating motion with a 2 kg roller, peel speed (tensile speed): 300 mm / min, peel angle 180°).

[0053] (Substrate) The substrate may be made of any appropriate material. For example, various sheet-like materials can be used as the substrate, such as plastic film, plastic sheet, paper, cloth, nonwoven fabric, metal foil, or plastic laminates thereof, or laminates of plastics. Among these, plastic film and plastic sheet (hereinafter referred to as plastic film) are most preferable from the viewpoints of handleability and cost. The material of the plastic film can be selected as needed from the viewpoints of strength, heat resistance, and the like. Examples of suitable materials include olefin-based resins containing α-olefins as monomer components, such as polyethylene (PE), polypropylene (PP), ethylene-propylene copolymer, and ethylene-vinyl acetate copolymer (EVA); polyesters, such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate (PBT); polyvinyl chloride (PVC); polyphenylene sulfide (PPS); amide-based resins, such as polyamide (nylon) and wholly aromatic polyamide (aramid); polyether ether ketone (PEEK), polyimide, polyetherimide, polystyrene, and acrylic resin. These materials can be used alone or in combination of two or more. The plastic film may be any of an unstretched film, a uniaxially oriented film, and a biaxially oriented film. These films may be laminated films consisting of two or more film layers, or, from the viewpoint of ease of handling, films containing a lubricant such as inert particles may be used.

[0054] In one embodiment, the substrate may function as a release liner.

[0055] The thickness of the substrate is preferably 200 μm or less, more preferably 1 μm to 200 μm, even more preferably 5 μm to 200 μm, particularly preferably 10 μm to 200 μm, particularly preferably 20 μm to 200 μm, and most preferably 30 μm to 200 μm.

[0056] The substrate may be subjected to a surface treatment, such as corona treatment, chromic acid treatment, ozone exposure, flame exposure, high-voltage shock exposure, ionizing radiation treatment, or coating with a primer.

[0057] (Pressure-sensitive adhesive layer) In one embodiment, the pressure-sensitive adhesive layer can be formed by applying the polyester-based pressure-sensitive adhesive to a substrate and curing the applied layer. That is, the pressure-sensitive adhesive layer can be a cured product of the polyester-based pressure-sensitive adhesive. The curing treatment is typically a crosslinking treatment. The curing treatment can be a curing treatment by heating or a curing treatment by active energy rays (e.g., ultraviolet rays). Curing conditions can be any appropriate conditions depending on the composition of the polyester-based pressure-sensitive adhesive.

[0058] The gel fraction of the pressure-sensitive adhesive layer (polyester-based pressure-sensitive adhesive after curing treatment) is preferably 50% to 95%, more preferably 60% to 90%, and even more preferably 70% to 80%. Within these ranges, a pressure-sensitive adhesive layer with excellent coatability and adhesive properties can be obtained. The method for measuring the gel fraction will be described later.

[0059] The glass transition temperature (Tg) of the pressure-sensitive adhesive layer (polyester-based pressure-sensitive adhesive after curing treatment) is preferably −100° C. to 0° C., more preferably −70° C. to −10° C., and even more preferably −60° C. to −20° C. Within such ranges, a pressure-sensitive adhesive layer excellent in both coatability and adhesiveness can be obtained. The Tg can typically be determined as the temperature corresponding to the peak top of the loss modulus G″ in dynamic viscoelasticity measurement performed at a frequency of 1 Hz. Specific measurement methods will be described later.

[0060] The thickness of the pressure-sensitive adhesive layer is preferably 5 μm to 200 μm, and more preferably 10 μm to 100 μm.

[0061] The haze value of the pressure-sensitive adhesive layer is preferably 0.1% to 5%, and more preferably 0.2% to 3%. Within this range, the transparency of the pressure-sensitive adhesive layer can be maintained.

[0062] (Method for producing pressure-sensitive adhesive sheet) The pressure-sensitive adhesive sheet can be produced by any appropriate method. Examples of the method for producing a pressure-sensitive adhesive sheet include a method of directly coating a substrate with a pressure-sensitive adhesive, and a method of coating a suitable substrate with a pressure-sensitive adhesive to form a coating layer and transferring the resulting coating layer to the substrate.

[0063] Examples of the method for applying the pressure-sensitive adhesive include coating methods using a die coater, a comma coater, a gravure coater, or the like.

[0064] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" are by weight unless otherwise specified. The methods for each evaluation are as follows.

[0065] (1) Weight average molecular weight A sample (polyester resin) was prepared in a 0.2 wt% tetrahydrofuran (THF) solution and left at room temperature for 20 hours. Then, it was filtered through a 0.45 μm membrane filter, and the filtrate was subjected to GPC measurement. Analytical device: Alliance manufactured by Waters Column: G7000HXL + GMHXL + GMHXL manufactured by Tosoh Column temperature: 40 ° C. Eluent: THF Flow rate: 0.8 mL / min Injection amount: 100 μL Detector: Differential refractometer (RI) Standard sample: Polystyrene (PS) manufactured by Agilent

[0066] (2) Viscosity The viscosity of the polyester-based pressure-sensitive adhesive was measured under the following conditions: Measuring device: HAAKE rheometer Cone plate: diameter 35 mm, 1°, made of titanium Shear rate: 0.1 to 1000 1 / s Temperature: 25°C Gap: 0.025 μm

[0067] (3) Contact angle A 2.0 μL drop of polyester-based pressure-sensitive adhesive (excluding the crosslinking agent and catalyst) was applied to the release-treated surface of a release-treated polyethylene terephthalate (PET) film, and the contact angle after 60 seconds was evaluated. The contact angle was measured using a contact angle meter (manufactured by Kyowa Interface Co., Ltd., product name "CX-A type") in an atmosphere of 23°C and 50% RH.

[0068] (4) Surface tension A syringe was filled with the polyester-based pressure-sensitive adhesive (compound excluding the crosslinking agent and catalyst) and set in a contact angle meter (manufactured by Kyowa Interface Co., Ltd., trade name "CX-A type"). In an atmosphere of 23°C and 50% RH, droplets of a size that would not fall were created, and the surface tension was evaluated by the pendant drop method.

[0069] (5) Adhesive Strength Sheet pieces measuring 100 mm in length and 20 mm in width were cut out from the pressure-sensitive adhesive sheets obtained in the Examples and Comparative Examples. Next, one release-treated PET film was peeled off from the pressure-sensitive adhesive sheet, and a PET film (trade name "Lumirror S10#25", manufactured by Toray Industries, Inc.) was attached (backed) to the exposed adhesive surface. Next, the other release-treated PET film was peeled off, and the sheet was pressed onto a SUS304 plate as a test plate using a 2 kg roller with one reciprocating motion, and left to stand in an atmosphere of 23°C and 50% RH for 72 hours. Thereafter, using a tensile tester (device name "EZ Test / Ez-S", manufactured by Shimadzu Corporation), the pressure-sensitive adhesive sheet (pressure-sensitive adhesive layer / PET film) was peeled off from the test plate in accordance with JIS Z0237 under conditions of an atmosphere of 23°C and 50% RH, a pulling rate of 300 mm / min, and a peel angle of 180°, and the adhesive strength (N / 20 mm) was measured.

[0070] (6) Coatability Coatability was evaluated based on the appearance of the pressure-sensitive adhesive sheets obtained in the Examples and Comparative Examples. ◯: No cissing △: Several cissings (within acceptable range) ×: Cracks present on the entire surface

[0071] [Production Example 1] Production of Polyester Resin A-1 In a reaction system equipped with a stirrer, thermometer, and outflow cooler, 1 mol of bis-2-hydroxyethyl terephthalate (manufactured by TCI) as the dicarboxylic acid component, 1.4 mol of dimer diol (trade name "Pripol 2033", molecular weight 534, manufactured by Croda Japan) as the diol component, 0.4 mol of polytetramethylene ether glycol (trade name "BioPTMG650", molecular weight 650), and 0.025 wt% of tetrabutyl titanate as the catalyst were charged, the pressure was reduced to 3 kPa, and condensation polymerization was carried out at 210 °C for 4 hours to obtain Polyester Resin A-1. This Polyester Resin A-1 had a weight average molecular weight Mw of 4,400 and a viscosity of 10 Pa s. The amounts of the dicarboxylic acid component and diol component used were such that 1.8 mol of hydroxyl groups were contained in the diol component per 1.0 mol of carboxyl groups contained in the dicarboxylic acid component.

[0072] [Production Example 2] Production of Polyester Resin A-2 In a reaction system equipped with a stirrer, thermometer, and outflow cooler, 1 mol of dimer acid (trade name "Pripol 1009", molecular weight 565, manufactured by Croda Japan) as a dicarboxylic acid component, 2 mol of polytetramethylene ether glycol (trade name "BioPTMG650", molecular weight 650) as a diol component, and 0.025 wt% of tetrabutyl titanate as a catalyst were charged, the pressure was reduced to 3 kPa, and condensation polymerization was carried out at 210 °C for 4 hours to obtain Polyester Resin A-2. This Polyester Resin A-2 had a weight average molecular weight Mw of 6,260 and a viscosity of 2.5 Pa s. The amounts of the dicarboxylic acid component and diol component used were such that 1.0 mol of carboxyl groups contained in the dicarboxylic acid component was replaced by 1.8 mol of hydroxyl groups contained in the diol component.

[0073] Example 1 A pressure-sensitive adhesive containing 100 parts by weight of polyester resin (A-1), 12 parts by weight of diisocyanate (trade name "Duranate D101", manufactured by Asahi Kasei) as a crosslinking agent, 8 parts by weight of polyisocyanate (trade name "Coronate HX", manufactured by Tosoh), 0.1 parts by weight of titanium tetraacetylacetonate as a catalyst, and 0.5 parts by weight of a silicone surfactant (trade name "BYK-329", manufactured by BYK Japan KK) as a surfactant was applied to the release-treated surface of a non-silicone release liner (trade name "PJ31", manufactured by Toray Industries, Inc.) so that the thickness after drying would be 20 μm, and the adhesive was heated at 130° C. for 1 minute and then left to stand in a 50° C. atmosphere for 3 days to obtain a pressure-sensitive adhesive sheet.

[0074] Example 2 A pressure-sensitive adhesive sheet was obtained in the same manner as in Example 1, except that the blending amount of the silicone surfactant was 1 part by weight.

[0075] Example 3 A pressure-sensitive adhesive sheet was obtained in the same manner as in Example 1, except that the blending amount of the silicone surfactant was changed to 3 parts by weight.

[0076] Example 4 A pressure-sensitive adhesive sheet was obtained in the same manner as in Example 1, except that polyester resin (A-2) was used instead of polyester resin (A-1).

[0077] Comparative Example 1 A pressure-sensitive adhesive sheet was obtained in the same manner as in Example 1, except that no silicone surfactant was added.

[0078]

[0079] 10 Pressure-sensitive adhesive layer 20 Substrate 100 Pressure-sensitive adhesive sheet

Claims

1. A polyester-based adhesive comprising a polyester-based resin and a surfactant, wherein the weight average molecular weight of the polyester-based resin is 0.2×10 4 ~2.0 x 10 4 The polyester-based pressure-sensitive adhesive has a viscosity of 1 Pa·s to 50 Pa·s.

2. The polyester-based pressure-sensitive adhesive according to claim 1, which is substantially free of organic solvents.

3. The polyester-based pressure-sensitive adhesive according to claim 1, wherein the surface tension of the polyester-based pressure-sensitive adhesive is 30 mN / m or less.

4. The polyester-based pressure-sensitive adhesive according to claim 1, wherein the polyester-based resin is a bio-polyester-based resin.

5. The polyester-based pressure-sensitive adhesive according to claim 1, wherein the surfactant is a silicone-based surfactant.

6. A method for producing a polyester-based pressure-sensitive adhesive, comprising: mixing a polyester-based resin with a surfactant to prepare a mixture, the mixture being substantially free of an organic solvent.

7. An adhesive sheet comprising an adhesive layer containing the polyester-based adhesive according to any one of claims 1 to 5.

8. The pressure-sensitive adhesive sheet according to claim 7, wherein the adhesive strength at 23° C. when the adhesive layer of the pressure-sensitive adhesive sheet is attached to a SUS304 plate is 5 N / 20 mm or more.

9. The pressure-sensitive adhesive sheet according to claim 7, wherein the haze value of the pressure-sensitive adhesive layer is 0.1% to 5%.

Citation Information

Patent Citations

  • Resin composition for adhesive and laminate using the same

    JP2003238930A

  • Double-sided adhesive tape

    JP2014169420A

  • Adhesive and adhesive sheet

    JP2019172813A

  • Polyester adhesive composition, polyester adhesive and adhesive sheet

    JP2020056006A

  • Polyester adhesive composition

    WO2011081163A1

Cited By

  • Pressure-sensitive adhesive sheet, laminate, and device

    WO2025205683A1