Method for producing pressure-sensitive adhesive sheet
The method of primary and secondary curing for a pressure-sensitive adhesive sheet using a polyester resin and acrylic resin composition addresses environmental concerns and coating defects, achieving effective adhesive strength and reduced solvent use.
Patent Information
- Application Number
- PCT/JP2024/009358
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-11
- Publication Date
- 2024-10-03
AI Technical Summary
The challenge is to produce a pressure-sensitive adhesive sheet with a polyester adhesive that reduces environmental impact while minimizing solvent use, as low molecular weight polyester resins can lead to coating defects and poor workability.
A method involving a coating step followed by primary curing with active energy rays and secondary curing by heating, using a polyester resin with a crosslinking agent and acrylic resin composition, which includes a photoreaction initiator, to form a pressure-sensitive adhesive layer without substantial organic solvents, thereby preventing coating defects.
This method enables the formation of a pressure-sensitive adhesive layer with reduced environmental impact and improved coating properties, preventing defects associated with low molecular weight polyester resins, while maintaining appropriate adhesive strength.
Smart Images

Figure JP2024009358_03102024_PF_FP_ABST
Abstract
Description
Method for manufacturing adhesive sheets
[0001] The present invention relates to a method for producing a pressure-sensitive adhesive sheet.
[0002] Pressure-sensitive adhesives have been used in various technical fields. In addition to acrylic pressure-sensitive adhesives, polyester pressure-sensitive adhesives have also been considered for use as pressure-sensitive adhesives from the viewpoint of optimizing adhesive strength.
[0003] On the other hand, the demand for reducing environmental impact is increasing year by year, and pressure sensitive adhesives are also being required to reduce environmental impact during production, use, etc.
[0004] JP 2020-056006 A JP 2003-238930 A
[0005] One way to reduce the environmental load is to reduce the amount of solvent used. However, when preparing a PSA with a low solvent content, it may be necessary to reduce the molecular weight of the base polymer (e.g., polyester resin) in the PSA, and the low molecular weight of the base polymer may cause deterioration in coatability and coating defects.
[0006] The present invention has been made to solve the above-mentioned conventional problems, and an object of the present invention is to provide a method for producing an adhesive sheet containing a polyester-based adhesive that can contribute to reducing the environmental load, and that can form an adhesive layer while preventing poor coating of the polyester-based adhesive.
[0007] [1] A method for producing a pressure-sensitive adhesive sheet according to one embodiment of the present invention includes a coating step of applying a polyester-based pressure-sensitive adhesive to a substrate to form a coating layer, a primary curing step of curing the coating layer with active energy rays to form a primary cured layer, and a secondary curing step of further curing the primary cured layer by heating after the primary curing step. The polyester-based pressure-sensitive adhesive includes a polyester-based resin, a crosslinking agent, an acrylic resin composition, and a photoinitiator. The acrylic resin composition includes an acrylic resin and a monomer component constituting the acrylic resin. [2] In the method for producing a pressure-sensitive adhesive sheet described in [1] above, the polyester-based pressure-sensitive adhesive may further include a polyfunctional acrylic monomer. [3] In the method for producing a pressure-sensitive adhesive sheet described in [1] or [2] above, the polyester-based pressure-sensitive adhesive may be substantially free of an organic solvent. [4] In the method for producing a pressure-sensitive adhesive sheet described in any one of [1] to [3] above, the content of the photoinitiator may be 0.001 parts by weight or more per 100 parts by weight of the polyester-based resin. [5] In the method for producing a pressure-sensitive adhesive sheet according to any one of [1] to [4] above, the polyester-based pressure-sensitive adhesive may further contain a crosslinking catalyst. [6] In the method for producing a pressure-sensitive adhesive sheet according to any one of [1] to [5] above, the heating temperature in the secondary curing step may be 90°C to 150°C.
[0008] According to the present invention, it is possible to provide a method for producing an adhesive sheet containing a polyester-based adhesive that can contribute to reducing the environmental load, and that can form an adhesive layer while preventing poor coating of the polyester-based adhesive.
[0009] 1A and 1B are schematic cross-sectional views of a pressure-sensitive adhesive sheet manufactured by a pressure-sensitive adhesive sheet manufacturing method according to one embodiment of the present invention.
[0010] A. Method for Producing a Pressure-Sensitive Adhesive Sheet A method for producing a pressure-sensitive adhesive sheet according to an embodiment of the present invention includes a coating step of applying a polyester-based pressure-sensitive adhesive to a substrate to form a coating layer, a primary curing step of curing the coating layer with active energy rays to form a primary cured layer, and a secondary curing step of further curing the primary cured layer by heating after the primary curing step.
[0011] In an embodiment of the present invention, by performing primary curing with active energy rays before heat curing, it is possible to reduce the change in viscosity of the adhesive coating layer due to heating during heat curing, and as a result, it is possible to prevent coating defects.
[0012] B. Coating Step B-1. Polyester-Based Pressure-Sensitive Adhesive The polyester-based pressure-sensitive adhesive contains a polyester resin, a crosslinking agent, an acrylic resin composition, and a photoinitiator. The acrylic resin composition contains an acrylic resin and a monomer component constituting the acrylic resin.
[0013] The present invention is advantageous in that it can prevent coating defects as described above while using a polyester resin having a low molecular weight. By using a polyester resin having a low molecular weight, the amount of organic solvent added can be reduced, resulting in a polyester pressure-sensitive adhesive with a low environmental impact.
[0014] Preferably, the polyester-based PSA is substantially free of organic solvents. By being substantially free of organic solvents, a polyester-based PSA with low environmental impact can be provided. The concept of "substantially free of organic solvents" (hereinafter also referred to as "solvent-free") can also encompass embodiments in which a small amount of organic solvent inevitably present in the raw materials or unintentionally mixed in during production is contained. However, the amount of unintentionally contained organic solvent is preferably 3 parts by weight or less, more preferably 1 part by weight or less, more preferably 0.5 parts by weight or less, and particularly preferably 0.1 parts by weight or less, per 100 parts by weight of the polyester-based PSA. When a low-molecular-weight polyester-based resin is used to prepare a solvent-free PSA, coating defects such as repelling may occur when the resin is applied to a substrate (such as a release liner) and cured by heating. However, in the present invention, such coating defects can be prevented by performing primary curing as described above.
[0015] The viscosity of the polyester-based pressure-sensitive adhesive at 25°C is preferably 2 Pa·s to 80 Pa·s, more preferably 4 Pa·s to 60 Pa·s, and even more preferably 5 Pa·s to 50 Pa·s. Within these ranges, a polyester-based pressure-sensitive adhesive with excellent coatability can be obtained. In this specification, viscosity refers to a viscosity at 0.1 to 1000 (1 / s) measured using a rheometer.
[0016] (Polyester Resin) Typically, polyester resins are obtained by reacting a polycarboxylic acid component with a polyhydric alcohol component. The polycarboxylic acid component contains one or more compounds selected from polycarboxylic acids having two or more carboxyl groups in one molecule and their derivatives. The polyhydric alcohol component contains one or more compounds selected from polyhydric alcohols having two or more hydroxyl groups in one molecule.
[0017] In one embodiment, the polyester resin is a biopolyester resin. In this specification, the biopolyester resin refers to a polyester resin in which at least one of a polycarboxylic acid component and a polyhydric alcohol component is derived from a plant. By using the renewable plant-derived material, it is possible to obtain a polyester pressure-sensitive adhesive that can address the depletion of fossil resources and global warming and contribute to reducing the environmental impact.
[0018] Examples of the polycarboxylic acid include aliphatic or alicyclic dibasic acids. Specific examples include adipic acid, azelaic acid, dimer acid, sebacic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 4-methyl-1,2-cyclohexanedicarboxylic acid, dodecenylsuccinic anhydride, fumaric acid, succinic acid, dodecanedioic acid, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, maleic acid, maleic anhydride, itaconic acid, and citraconic acid. Aromatic dibasic acids may also be used. Specific examples of aromatic dibasic acids include terephthalic acid, isophthalic acid, orthophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 2,2'-diphenyldicarboxylic acid, and 4,4'-diphenyletherdicarboxylic acid. As the polycarboxylic acid derivative, anhydrides and alkyl esters (for example, monoesters, diesters, etc., preferably monoalcohols having 1 to 3 carbon atoms) of the above carboxylic acids can be used.
[0019] In one embodiment, a plant-derived polycarboxylic acid is used. Examples of plant-derived polycarboxylic acids include dimer acid, sebacic acid, succinic acid, and glutaric acid. Here, "dimer acid" refers to a dicarboxylic acid having a structure in which an unsaturated fatty acid is dimerized. A typical example of the dimer acid is a dicarboxylic acid having 36 carbon atoms and a structure in which an unsaturated fatty acid having 18 carbon atoms (oleic acid, linoleic acid, linolenic acid, etc.) is dimerized.
[0020] When the polycarboxylic acid component contains a plant-derived polycarboxylic acid, the content of the plant-derived polycarboxylic acid is preferably 10 mol % or more, preferably 50 mol % or more, more preferably 75 mol % or more, even more preferably 90 mol % or more, and most preferably 100 mol % based on the total amount of polycarboxylic acids in the polycarboxylic acid component.
[0021] Examples of the polyhydric alcohol include aliphatic or alicyclic diols, such as ethylene glycol, 1,2-propylene glycol, 1,3-propanediol, 2-methyl-1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, diethylene glycol, dipropylene glycol, 2,2,4-trimethyl-1,5-pentanediol, 2-ethyl-2-butylpropanediol, 1,9-nonanediol, 2-methyloctanediol, and 1,10-decanediol.
[0022] In one embodiment, a plant-derived polyhydric alcohol is used. Examples of plant-derived polyhydric alcohols include dimer diol, 1,3-propanediol, 1,4-butanediol, ethylene glycol, and polyoxytetramethylene glycol. Here, "dimer diol" refers to a diol having a structure in which the carboxyl group in a dicarboxylic acid formed by dimerization of an unsaturated fatty acid is converted to a hydroxyl group (hydrogenated). A diol having 36 carbon atoms corresponding to a dimer of an unsaturated fatty acid having 18 carbon atoms (oleic acid, linoleic acid, linolenic acid, etc.) is a typical example included in the above dimer diol.
[0023] When the polyhydric alcohol component contains a plant-derived polyhydric alcohol, the content of the plant-derived polyhydric alcohol is preferably 50 mol% or more, more preferably 75 mol% or more, even more preferably 90 mol% or more, and most preferably 100 mol% relative to the total polyhydric alcohols in the polyhydric alcohol component.
[0024] The polyester resin can be obtained by polycondensation of a polycarboxylic acid component and a polyhydric alcohol component. More specifically, the polyester resin can be produced (synthesized) by proceeding with the condensation reaction between a carboxyl group of the polycarboxylic acid component and a hydroxyl group of the polyhydric alcohol component, for example, while removing water (condensed water) produced by the condensation reaction from the reaction system. Methods for removing the condensed water from the reaction system include a method of blowing an inert gas into the reaction system and removing the condensed water together with the inert gas from the reaction system, and a method of distilling off the condensed water from the reaction system under reduced pressure (reduced pressure method). The reduced pressure method is preferably used because it is suitable for shortening the polymerization time and improving productivity.
[0025] The reaction conditions, such as the reaction temperature when carrying out the condensation reaction and the degree of vacuum (pressure in the reaction system) when a reduced pressure method is adopted, can be any appropriate conditions. The reaction temperature is, for example, 180°C to 260°C, and preferably 200°C to 220°C. The degree of vacuum is, for example, 10 kPa or less, preferably 0.1 kPa to 10 kPa, and more preferably 0.1 kPa to 4 kPa.
[0026] Any appropriate polymerization catalyst may be used in the condensation reaction. Examples of the polymerization catalyst include titanium-based catalysts such as tetraisopropyl titanate and tetrabutyl titanate, antimony-based catalysts such as antimony trioxide, germanium-based catalysts such as germanium dioxide, and catalysts such as zinc acetate, manganese acetate, and dibutyltin oxide. These catalysts may be used alone or in combination of two or more. Among these, antimony trioxide, tetrabutyl titanate, germanium dioxide, and zinc acetate are preferably used.
[0027] The amount of the polymerization catalyst may be any appropriate amount, and is, for example, preferably 0.001 mol % to 5 mol %, more preferably 0.01 mol % to 3 mol %, and even more preferably 0.1 mol % to 2 mol %, based on the total amount of the polycarboxylic acid component and the polyhydric alcohol component.
[0028] In one embodiment, the synthesis of the polyester resin can be carried out without using an organic solvent.
[0029] The content of the polyester resin is preferably 60 parts by weight or more, more preferably 70 parts by weight or more, and even more preferably 80 parts by weight or more, based on 100 parts by weight of the polyester pressure-sensitive adhesive.
[0030] The weight average molecular weight of the polyester resin is preferably 0.2×10 4 ~2.0 x 10 4 Within this range, a polyester-based pressure-sensitive adhesive that can exhibit appropriate adhesive strength can be preferably prepared without containing a solvent. The weight-average molecular weight of the polyester-based resin is more preferably 0.25 × 10 4 ~1.5 x 10 4 and more preferably 0.3 × 10 4 ~1.0 x 10 4 Within this range, the above-mentioned effects become significant. In this specification, the weight average molecular weight refers to a value calculated in terms of polystyrene measured by gel permeation chromatography (GPC).
[0031] (Crosslinking Agent) As described above, the polyester-based pressure-sensitive adhesive contains a crosslinking agent. In one embodiment, an isocyanate-based crosslinking agent and / or an epoxy-based crosslinking agent is used as the crosslinking agent. In one embodiment, the content of the crosslinking agent is 3 parts by weight or more relative to 100 parts by weight of the polyester-based resin.
[0032] The isocyanate crosslinking agent is a compound having an isocyanate group, and specific examples thereof include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate; aromatic isocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate and xylylene diisocyanate; and isocyanate adducts such as trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., trade name "Coronate L"), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., trade name "Coronate HL"), and isocyanurate of hexamethylene diisocyanate (manufactured by Nippon Polyurethane Industry Co., Ltd., trade name "Coronate HX"). When the polyester-based pressure-sensitive adhesive contains an isocyanate-based crosslinking agent, the content of the isocyanate-based crosslinking agent can be set to any appropriate amount depending on the desired adhesive strength, and is preferably 3 to 30 parts by weight, more preferably 10 to 20 parts by weight, relative to 100 parts by weight of the polyester-based resin.
[0033] The epoxy crosslinking agent is a compound having an epoxy group, and specific examples thereof include N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, 1,3-bis(N,N-glycidylaminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Company, Inc., trade name "Tetrad C"), 1,6-hexanediol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 1600"), neopentyl glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 1500N"), and 1,6-hexanediol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 1500N"). P"), ethylene glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 40E"), propylene glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., trade name "Epolite 70P"), polyethylene glycol diglycidyl ether (manufactured by NOF Corporation, trade name "Epiol E-400"), polypropylene glycol diglycidyl ether (manufactured by NOF Corporation, trade name "Epiol P-200"), sorbitol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol" EX-611), glycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol EX-314"), pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol EX-512"), sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. When the polyester-based pressure-sensitive adhesive contains an epoxy-based crosslinking agent, the content of the epoxy-based crosslinking agent can be set to any appropriate amount depending on the desired adhesive strength, and is typically 0.01 to 10 parts by weight, and more preferably 3 to 5 parts by weight, relative to 100 parts by weight of the polyester-based resin.
[0034] (Acrylic Resin Composition) As described above, the acrylic resin composition contains an acrylic resin and a monomer component constituting the acrylic resin. In the acrylic resin composition, the polymerization rate of the polymer is less than 100% (e.g., 5% to 10%). Therefore, the acrylic resin composition may further contain a monomer component (raw material) constituting the remaining acrylic resin.
[0035] In one embodiment, the acrylic resin composition further contains a polyfunctional acrylic monomer. In this embodiment, the acrylic resin composition can be prepared, for example, by adding the polyfunctional acrylic monomer to a mixture of an acrylic resin and a residual monomer (a monomer component (raw material) constituting the acrylic resin) after polymerization of the acrylic resin. In other words, the polyfunctional acrylic monomer is different from the monomer component constituting the acrylic resin.
[0036] The viscosity of the acrylic resin composition is, for example, 10 Pa·s to 20 Pa·s.
[0037] In one embodiment, the acrylic resin is a polymer of a monomer raw material containing, for example, an alkyl(meth)acrylate as a main monomer and a secondary monomer copolymerizable with the main monomer. Here, the main monomer refers to a component that accounts for more than 50% by weight of the monomer composition in the monomer raw material. The content of the main monomer is preferably 60 to 100 parts by weight, more preferably 70 to 99.5 parts by weight, per 100 parts by weight of the total amount of monomers in the monomer raw material.
[0038] As the alkyl(meth)acrylate, for example, a compound represented by the following formula (1) can be suitably used: CH 2 = C(R 1 ) COOR 2 (1) Here, R in the above formula (1) 1 is a hydrogen atom or a methyl group. 2 is a branched or linear alkyl group having 1 to 20 carbon atoms (hereinafter, this range of carbon atoms may be referred to as "C1-20"). 2is preferably a branched or straight-chain C1-14 alkyl group, more preferably a branched or straight-chain C4-14 alkyl group, and even more preferably a branched or straight-chain C4-8 alkyl group.
[0039] Specific examples of the alkyl(meth)acrylate include methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, isopropyl(meth)acrylate, n-butyl(meth)acrylate, isobutyl(meth)acrylate, s-butyl(meth)acrylate, pentyl(meth)acrylate, isopentyl(meth)acrylate, hexyl(meth)acrylate, heptyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, octyl(meth)acrylate, and isooctyl(meth)acrylate. ) acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, etc. These alkyl (meth)acrylates can be used alone or in combination of two or more.
[0040] The secondary monomer copolymerizable with the alkyl(meth)acrylate main monomer can be useful for introducing crosslinking points into the acrylic polymer and for increasing the cohesive strength of the acrylic polymer. As the secondary monomer, for example, the following functional group-containing monomer components can be used alone or in combination of two or more: Carboxy group-containing monomers: for example, ethylenically unsaturated monocarboxylic acids such as acrylic acid (AA), methacrylic acid (MAA), crotonic acid, etc.; ethylenically unsaturated dicarboxylic acids such as maleic acid, itaconic acid, citraconic acid, etc., and anhydrides thereof (maleic anhydride, itaconic anhydride, etc.); hydroxyl group-containing monomers: for example, hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, etc.; unsaturated alcohols such as vinyl alcohol, allyl alcohol, etc.; ether compounds such as 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, diethylene glycol monovinyl ether, etc.; amino group-containing monomers: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, t-butylaminoethyl (meth)acrylate; epoxy group-containing monomers: for example, glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, allyl glycidyl ether; Cyano group-containing monomers: for example, acrylonitrile, methacrylonitrile; keto group-containing monomers: for example, diacetone (meth)acrylamide, diacetone (meth)acrylate, vinyl methyl ketone, vinyl ethyl ketone, allyl acetoacetate, vinyl acetoacetate; monomers having a nitrogen atom-containing ring: for example, N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-vinylmorpholine, N-vinylcaprolactam, N-(meth)acryloylmorpholine;Alkoxysilyl group-containing monomers: for example, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane; Isocyanate group-containing monomers: (meth)acryloyl isocyanate, 2-(meth)acryloyloxyethyl isocyanate, m-isopropenyl-α,α-dimethylbenzyl isocyanate;
[0041] The content of the structural unit derived from the functional group-containing monomer is preferably 0.01 to 40 parts by weight, more preferably 0.03 to 20 parts by weight, per 100 parts by weight of the total amount of monomers in the monomer raw material.
[0042] Copolymerization components other than the functional group-containing monomers described above can also be used. Examples of such copolymerization components include vinyl ester-based monomers such as vinyl acetate and vinyl propionate; aromatic vinyl compounds such as styrene, substituted styrenes (such as α-methylstyrene), and vinyltoluene; cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate, cyclopentyl di(meth)acrylate, and isobornyl (meth)acrylate; aromatic ring-containing (meth)acrylates such as aryl (meth)acrylates (such as phenyl (meth)acrylate), aryloxyalkyl (meth)acrylates (such as phenoxyethyl (meth)acrylate), and arylalkyl (meth)acrylates (such as benzyl (meth)acrylate); olefin-based monomers such as ethylene, propylene, isoprene, butadiene, and isobutylene; chlorine-containing monomers such as vinyl chloride and vinylidene chloride; alkoxy group-containing monomers such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; vinyl ether-based monomers such as methyl vinyl ether and ethyl vinyl ether; and the like. The copolymerization components other than these secondary monomers may be used alone or in combination of two or more thereof. The amount of such copolymerization components is, for example, 0.1 to 20 parts by weight per 100 parts by weight of the total amount of monomers in the monomer raw material.
[0043] The polyfunctional acrylic monomer may be, for example, an acrylic monomer having at least two polymerizable functional groups (typically radically polymerizable functional groups) having an unsaturated double bond, such as a (meth)acryloyl group or a vinyl group. Use of the polyfunctional acrylic monomer can increase the cohesive strength of the pressure-sensitive adhesive layer.
[0044] Examples of polyfunctional acrylic monomers include ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,2-ethylene glycol di(meth)acrylate, 1,4-butanediol, Examples of suitable acrylic monomers include esters of polyhydric alcohols and (meth)acrylic acid, such as allyl di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and tetramethylolmethane tri(meth)acrylate; allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, and urethane acrylate. Among these, preferred examples include trimethylolpropane tri(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, and dipentaerythritol hexa(meth)acrylate. Of these, preferred examples include dipentaerythritol hexa(meth)acrylate. The polyfunctional acrylic monomers can be used singly or in combination of two or more. In view of reactivity and the like, polyfunctional acrylic monomers having two or more acryloyl groups are usually preferred.
[0045] The amount of polyfunctional acrylic monomer used (added amount) is preferably 0.001 to 2 parts by weight, more preferably 0.01 to 1 part by weight, and even more preferably 0.05 to 0.5 parts by weight, relative to 100 parts by weight of the acrylic resin composition. Within such a range, a primary cured layer having a preferred viscosity can be formed, resulting in remarkable effects of the present invention.
[0046] The content of the acrylic resin composition is preferably 1 to 30 parts by weight, more preferably 2 to 20 parts by weight, and even more preferably 3 to 10 parts by weight, relative to 100 parts by weight of the polyester resin. Within such a range, a primary cured layer with a preferred viscosity can be formed, resulting in significant effects of the present invention. In one embodiment, the content of the acrylic resin composition is 20 parts by weight or less relative to 100 parts by weight of the polyester resin.
[0047] (Photoinitiator) Any appropriate initiator can be used as the photoinitiator. Examples of the photoinitiator include α-ketol compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α'-dimethylacetophenone, 2-methyl-2-hydroxypropiophenone, and 1-hydroxycyclohexylphenyl ketone; acetophenone compounds such as methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, and 2-methyl-1-[4-(methylthio)-phenyl]-2-morpholinopropane-1; benzoin ether compounds such as benzoin ethyl ether, benzoin isopropyl ether, and anisoin methyl ether; and ketal compounds such as benzyl dimethyl ketal. aromatic sulfonyl chloride compounds such as 2-naphthalenesulfonyl chloride; photoactive oxime compounds such as 1-phenone-1,1-propanedione-2-(o-ethoxycarbonyl)oxime; benzophenone compounds such as benzophenone, benzoylbenzoic acid, and 3,3'-dimethyl-4-methoxybenzophenone; thioxanthone compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, and 2,4-diisopropylthioxanthone; camphorquinone; halogenated ketones; acylphosphinoxides; and acylphosphonates. The amount of the photoreaction initiator used can be set to any appropriate amount.
[0048] The content of the photoreaction initiator is preferably 0.001 part by weight or more, more preferably 0.002 part by weight or more, and even more preferably 0.005 part by weight or more, based on 100 parts by weight of the polyester resin.
[0049] (Other Additives) The polyester-based pressure-sensitive adhesive may further contain any appropriate additives as necessary. Examples of additives include tackifiers, plasticizers (e.g., trimellitic ester-based plasticizers, pyromellitic ester-based plasticizers, etc.), pigments, dyes, fillers, antioxidants, conductive materials, antistatic agents, UV absorbers, light stabilizers, release adjusters, softeners, surfactants, flame retardants, antioxidants, etc. The polyester-based pressure-sensitive adhesive may also further contain other resins such as acrylic resins, natural rubber resins, synthetic rubber resins, and silicone resins.
[0050] In one embodiment, the polyester-based pressure-sensitive adhesive contains a crosslinking catalyst. Examples of the crosslinking catalyst include metal complex compounds such as aluminum triacetylacetonate, iron triacetylacetonate, manganese tetraacetylacetonate, nickel tetraacetylacetonate, chromium hexaacetylacetonate, titanium tetraacetylacetonate, and cobalt tetraacetylacetonate; metal alkoxides such as aluminum ethoxide, aluminum propoxide, aluminum butoxide, titanium ethoxide, titanium propoxide, and titanium butoxide; metal salt compounds such as sodium acetate, tin octoate, lead octoate, cobalt octoate, zinc octoate, calcium octoate, lead naphthenate, cobalt naphthenate, dibutyltin dioctate, dibutyltin dilaurate, dibutyltin maleate, and dibutyltin di(2-ethylhexoate); formic acid, acetic acid, propionic acid, and p-toluenesulfonyl ether. acidic compounds such as toluenesulfonic acid, trichloroacetic acid, phosphoric acid, monoalkyl phosphoric acid, dialkyl phosphoric acid, phosphate ester of β-hydroxyethyl (meth)acrylate, monoalkyl phosphorous acid, dialkyl phosphorous acid; acids such as p-toluenesulfonic acid, phthalic anhydride, benzoic acid, benzenesulfonic acid, dodecylbenzenesulfonic acid, formic acid, acetic acid, itaconic acid, oxalic acid, maleic acid, and the like; and ammonium salts, lower amine salts, polyvalent metal salts thereof; organometallic compounds such as sodium hydroxide, lithium chloride, diethylzinc, and tetra(n-butoxy)titanium; and amines such as dicyclohexylamine, triethylamine, N,N-dimethylbenzylamine, N,N,N',N'-tetramethyl-1,3-butanediamine, diethanolamine, triethanolamine, and cyclohexylethylamine.
[0051] The content of the crosslinking catalyst is preferably 0.01 to 1 part by weight, more preferably 0.05 to 0.8 parts by weight, and even more preferably 0.08 to 0.5 parts by weight, relative to 100 parts by weight of the polyester resin. Within such a range, a polyester pressure-sensitive adhesive that prevents coating defects can be obtained.
[0052] In one embodiment, the polyester-based PSA contains a surfactant. By adding the surfactant, the surface tension of the polyester-based PSA can be preferably adjusted, and as a result, a polyester-based PSA with excellent coatability can be obtained.
[0053] In one embodiment, the polyester-based pressure-sensitive adhesive contains inorganic particles. The inorganic particles may be inorganic particles that can impart thixotropy to the polyester-based pressure-sensitive adhesive.
[0054] Examples of the inorganic particles include silica, titanium dioxide, bentonite, zinc oxide, talc, kaolin, mica, vermiculite, magnesium carbonate, calcium carbonate, aluminum silicate, barium silicate, calcium silicate, magnesium silicate, strontium silicate, metal tungstate, magnesium, zeolite, barium sulfate, calcined calcium sulfate, calcium phosphate, fluorapatite, hydroxyapatite, and metal soap. Composite particles obtained by coating particles with a metal oxide or the like, or modified particles whose particle surfaces have been treated with a compound or the like, may also be used. Among these, silica particles are preferably used, and fumed silica is more preferably used.
[0055] The content of the inorganic particles is preferably 1 to 30 parts by weight, more preferably 3 to 20 parts by weight, and even more preferably 3 to 10 parts by weight, relative to 100 parts by weight of the polyester resin. Within such a range, a polyester pressure-sensitive adhesive that prevents coating defects can be obtained.
[0056] (Method for producing polyester-based pressure-sensitive adhesive) In one embodiment, a method for producing a polyester-based pressure-sensitive adhesive includes mixing a polyester-based resin, a crosslinking agent, an acrylic resin, a monomer component used in polymerization of the acrylic resin (a monomer component constituting the acrylic resin), other components added as needed (e.g., a polyfunctional acrylic monomer), and a photoinitiator to prepare a mixture, and is characterized in that the mixture does not substantially contain organic matter.
[0057] In one embodiment, the polyester-based resin used in the above production method is the polyester-based resin described in the above section A. However, in the above production method, the polyester-based resin has a weight-average molecular weight of 0.2 × 10 4 ~2.0 x 10 4 In place of such a polyester resin, a polyester resin having a molecular weight outside the above range may be used as long as the effects of the present invention can be obtained.
[0058] The crosslinking agent, acrylic resin, polyfunctional acrylic monomer, and photoinitiator may be those described above. The mixture may further contain the additives described above (e.g., crosslinking catalyst).
[0059] B-2. Substrate The substrate can be made of any appropriate material. The substrate can be, for example, a plastic film, a plastic sheet, or various sheet-like materials such as paper, cloth, nonwoven fabric, metal foil, or plastic laminates thereof, or laminates of plastics. Among these, plastic films and plastic sheets (hereinafter referred to as plastic films) are most preferable from the standpoints of handleability and cost. The material for the plastic film can be selected as needed from the standpoints of strength, heat resistance, and the like. Examples of suitable materials include olefin-based resins containing α-olefins as monomer components, such as polyethylene (PE), polypropylene (PP), ethylene-propylene copolymer, and ethylene-vinyl acetate copolymer (EVA); polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate (PBT); polyvinyl chloride (PVC); polyphenylene sulfide (PPS); amide-based resins such as polyamide (nylon) and wholly aromatic polyamide (aramid); polyether ether ketone (PEEK), polyimide, polyetherimide, polystyrene, and acrylic resins. These materials can be used alone or in combination of two or more. The plastic film may be any of an unstretched film, a uniaxially oriented film, and a biaxially oriented film. These films may be laminated films consisting of two or more film layers, or, from the viewpoint of ease of handling, films containing a lubricant such as inert particles may be used.
[0060] In one embodiment, the substrate may function as a release liner.
[0061] The substrate may or may not be an element of the pressure-sensitive adhesive sheet. That is, the pressure-sensitive adhesive sheet may be composed of only the pressure-sensitive adhesive layer, or may include the pressure-sensitive adhesive layer and the substrate. A pressure-sensitive adhesive sheet composed of only the pressure-sensitive adhesive layer can be obtained by forming the pressure-sensitive adhesive layer and then peeling off the substrate.
[0062] The thickness of the substrate is preferably 200 μm or less, more preferably 1 μm to 200 μm, even more preferably 5 μm to 200 μm, particularly preferably 10 μm to 200 μm, particularly preferably 20 μm to 200 μm, and most preferably 30 μm to 200 μm.
[0063] In one embodiment, the substrate has a light transmittance of 50% or more at a wavelength of 365 nm, preferably 80% or more, and more preferably 90% or more, and the upper limit of the light transmittance is, for example, 98% (preferably 100%).
[0064] The substrate may be subjected to a surface treatment, such as corona treatment, chromic acid treatment, ozone exposure, flame exposure, high-voltage shock exposure, ionizing radiation treatment, or coating with a primer.
[0065] B-3. Coating Method Any appropriate method can be used as a method for coating the polyester-based pressure-sensitive adhesive. Examples of the method for coating the polyester-based pressure-sensitive adhesive include coating methods using a die coater, a comma coater, a gravure coater, etc.
[0066] The thickness of the coating layer is preferably 5 μm to 100 μm, more preferably 8 μm to 50 μm, and even more preferably 10 μm to 30 μm.
[0067] C. Primary Curing Step As described above, the coating layer is cured with active energy rays to form a primary cured layer. In one embodiment, this step promotes polymerization of the remaining monomer components in the coating layer, i.e., the "monomer components constituting the acrylic resin." Furthermore, when the polyester-based pressure-sensitive adhesive contains the above-mentioned polyfunctional acrylic monomer, the primary curing step produces a polymer of the acrylic resin and the polyfunctional acrylic monomer.
[0068] Examples of active energy rays include gamma rays, ultraviolet rays, visible light, infrared rays (heat rays), radio waves, alpha rays, beta rays, electron beams, plasma flow, ionizing rays, particle beams, etc. Among these, ultraviolet rays are preferred.
[0069] In one embodiment, the irradiation of active energy rays has an integrated light dose of 500 mJ / cm 2 ~3000mJ / cm 2 (Preferably, 800 mJ / cm 2 ~2500mJ / cm 2 ) ultraviolet light (wavelength: using a high-pressure mercury lamp centered at 365 nm).
[0070] In one embodiment, the surface of the coating layer opposite the substrate is covered with an ultraviolet-transmitting film (a cover release film), and then the coating layer is irradiated with active energy rays. In this way, curing is preferably promoted and coating defects are prevented. The ultraviolet-transmitting film preferably has a light transmittance of 50% or more at a wavelength of 365 nm, preferably 80% or more, and more preferably 90% or more. The upper limit of the light transmittance is, for example, 98% (preferably 100%).
[0071] The thickness of the primary hardened layer is preferably 5 μm to 100 μm, more preferably 8 μm to 50 μm, and even more preferably 10 μm to 30 μm.
[0072] In one embodiment, after the primary cured layer is formed, a predetermined time is allowed to pass before the subsequent secondary curing step is carried out. When irradiating with active energy rays after covering with an ultraviolet-transmitting film, by carrying out the secondary curing after the predetermined time has passed, damage to the cured layer when peeling off the ultraviolet-transmitting film (the so-called "break-up phenomenon") can be prevented. The time from the formation of the primary cured layer until the secondary curing step is carried out is, for example, 3 hours to 48 hours, preferably 5 hours to 12 hours.
[0073] D. Secondary Curing Step As described above, in the secondary curing step, the primary cured layer is further cured by heating. A pressure-sensitive adhesive layer is formed by the secondary curing by heating.
[0074] The heating temperature is, for example, 80° C. to 160° C., and preferably 90° C. to 150° C. The heating time is, for example, 0.5 minutes to 5 minutes, and more preferably 1 minute to 3 minutes.
[0075] In one embodiment, in the primary curing step, the coating is covered with an ultraviolet-transmitting film, and then irradiated with active energy rays, and the film is then peeled off, followed by heating. In this way, the effect of preventing coating defects is significant.
[0076] E. Pressure-Sensitive Adhesive Sheet In one embodiment, a pressure-sensitive adhesive sheet is provided, which includes a pressure-sensitive adhesive layer formed from the polyester-based pressure-sensitive adhesive. Figure 1 is a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to one embodiment of the present invention. The pressure-sensitive adhesive sheet 100 may be composed of only a pressure-sensitive adhesive layer 10, as shown in Figure 1(a), or may be composed of a substrate 20 and a pressure-sensitive adhesive layer 10 disposed on at least one side of the substrate 20, as shown in Figure 1(b).
[0077] The thickness of the pressure-sensitive adhesive sheet is preferably 3 μm to 300 μm, more preferably 5 μm to 150 μm, and even more preferably 10 μm to 100 μm.
[0078] The adhesive strength at 23°C when the adhesive layer of the pressure-sensitive adhesive sheet is attached to an SUS304 plate is not particularly limited and can be adjusted to an appropriate range depending on the purpose and application. The initial adhesive strength may be, for example, 0.5 N / 20 mm or more, or 0.8 N / 20 mm or more. A pressure-sensitive adhesive sheet exhibiting an initial adhesive strength of a predetermined value or more can adhere well to an adherend. From this perspective, in some embodiments, the initial adhesive strength is preferably 1.0 N / 20 mm or more, more preferably 1.5 N / 20 mm or more, even more preferably 2.0 N / 20 mm or more, and may be 2.5 N / 20 mm or more, 3.0 N / 20 mm or more, 3.5 N / 20 mm or more, 4.0 N / 20 mm or more, or 4.5 N / 20 mm or more. The upper limit of the initial adhesive strength is not particularly limited and may be, for example, less than 30 N / 20 mm, or may be 25 N / 20 mm or less, 20 N / 20 mm or less, or 15 N / 20 mm or less from the viewpoint of easily balancing with other properties, etc. The adhesive strength refers to the adhesive strength measured by a method in accordance with JIS Z 0237:2009 (lamination conditions: one reciprocating motion with a 2 kg roller, peel speed (tensile speed): 300 mm / min, peel angle 180°).
[0079] The gel fraction of the pressure-sensitive adhesive layer (polyester-based pressure-sensitive adhesive after curing treatment) is preferably 50% to 95%, more preferably 60% to 90%, and even more preferably 70% to 80%. Within these ranges, a pressure-sensitive adhesive layer with excellent coatability and adhesive properties can be obtained. The method for measuring the gel fraction is as follows.
[0080] Gel fraction: Approximately 0.1 g of the pressure-sensitive adhesive layer was sampled and wrapped in a porous tetrafluoroethylene sheet (trade name "NTF1122", manufactured by Nitto Denko Corporation) having an average pore size of 0.2 μm, and then tied with kite string. The weight at this time was measured and this weight was defined as the weight before immersion (Z). The weight before immersion is the total weight of the pressure-sensitive adhesive layer (the pressure-sensitive adhesive layer sampled above), the tetrafluoroethylene sheet, and the kite string. The total weight of the tetrafluoroethylene sheet and the kite string was also measured, and this weight was defined as the bag weight (Y). Next, the pressure-sensitive adhesive layer wrapped in the tetrafluoroethylene sheet and tied with the kite string (referred to as the "sample") was placed in a 50 ml container filled with toluene and allowed to stand at 23° C. for 7 days. The sample (after toluene treatment) was then removed from the container and transferred to an aluminum cup. It was then dried in a dryer at 130°C for 2 hours to remove the toluene, and its weight was measured. This weight was taken as the post-immersion weight (X). The gel fraction was calculated using the following formula: Gel fraction [% (wt%)] = (X-Y) / (Z-Y) x 100
[0081] The glass transition temperature (Tg) of the pressure-sensitive adhesive layer (polyester-based pressure-sensitive adhesive after curing treatment) is preferably −100° C. to 0° C., more preferably −70° C. to −10° C., and even more preferably −60° C. to −20° C. Within such a range, a pressure-sensitive adhesive layer having excellent coatability and adhesive properties can be obtained. The Tg can be determined as the temperature corresponding to the peak top of the loss modulus G″ in dynamic viscoelasticity measurement performed at a frequency of 1 Hz.
[0082] The thickness of the pressure-sensitive adhesive layer is preferably 5 μm to 200 μm, and more preferably 10 μm to 100 μm.
[0083] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" are by weight unless otherwise specified. The methods for each evaluation are as follows.
[0084] (1) Weight average molecular weight A sample (polyester resin) was prepared in a 0.2 wt% tetrahydrofuran (THF) solution and left at room temperature for 20 hours. Then, it was filtered through a 0.45 μm membrane filter, and the filtrate was subjected to GPC measurement. Analytical device: Alliance manufactured by Waters Column: G7000HXL + GMHXL + GMHXL manufactured by Tosoh Column temperature: 40 ° C. Eluent: THF Flow rate: 0.8 mL / min Injection amount: 100 μL Detector: Differential refractometer (RI) Standard sample: Polystyrene (PS) manufactured by Agilent
[0085] (2) Viscosity The viscosity of the polyester-based pressure-sensitive adhesive was measured under the following conditions: Measuring device: HAAKE rheometer Cone plate: diameter 35 mm, 1°, made of titanium Shear rate: 0.1 to 1000 1 / s Temperature: 25°C Gap: 0.025 μm
[0086] (3) Coatability Coatability was evaluated based on the appearance of the pressure-sensitive adhesive sheets obtained in the Examples and Comparative Examples. ◯: No cissing ×: Cracks present
[0087] (4) Separation Separation was evaluated based on the appearance of the adhesive sheet when the cover release film of the adhesive sheet was peeled off after primary curing in the examples and comparative examples. ○: No separation ×: Separation
[0088] [Production Example 1] Production of Polyester Resin In a reaction system equipped with a stirrer, thermometer, and outflow cooler, 1 mol of bis-2-hydroxyethyl terephthalate (manufactured by TCI) as the dicarboxylic acid component, 1.4 mol of dimer diol (trade name "Pripol 2033", molecular weight 534, manufactured by Croda Japan) as the diol component, 0.4 mol of polytetramethylene ether glycol (trade name "BioPTMG650", molecular weight 650), and 0.025 wt% of tetrabutyl titanate as the catalyst were charged, the pressure was reduced to 3 kPa, and condensation polymerization was carried out at 210 °C for 4 hours to obtain Polyester Resin A-1. This Polyester Resin A-1 had a weight average molecular weight Mw of 4,400 and a viscosity of 10 Pa s. The amounts of the dicarboxylic acid component and diol component used were such that 1.8 mol of hydroxyl groups were contained in the diol component per 1.0 mol of carboxyl groups contained in the dicarboxylic acid component.
[0089] [Production Example 2] Production of acrylic resin To a monomer mixture consisting of 99 parts by weight of heptyl acrylate (HpA) and 1 part by weight of 4-hydroxybutyl acrylate (4HBA), 0.05 parts by weight of 1-hydroxycyclohexyl phenyl ketone (BASF "Irgacure 184") and 0.05 parts by weight of 2,2-dimethoxy-1,2-diphenylethan-1-one (BASF "Irgacure 651") were added as photoinitiators. This composition was irradiated with ultraviolet light and prepolymerized until the viscosity at room temperature reached approximately 20 Pa s, yielding Composition B-1 containing an acrylic resin with a polymerization rate of approximately 7%.
[0090] [Example 1] A pressure-sensitive adhesive containing 100 parts by weight of polyester resin A-1, 5 parts by weight of composition B-1 containing acrylic resin, 0.01 parts by weight of dipentaerythritol hexaacrylate (DPHA), 12 parts by weight of diisocyanate (trade name "Duranate D101", manufactured by Asahi Kasei) as a crosslinking agent, 8 parts by weight of polyisocyanate (trade name "Coronate HX", manufactured by Tosoh), and 0.1 parts by weight of titanium tetraacetylacetonate as a catalyst was applied to the release-treated surface of a substrate (silicone release liner, manufactured by Mitsubishi Chemical Corporation, trade name "MRF38") to a thickness of 20 μm, and a cover release film was attached to the surface of the coating layer to obtain a laminate. This laminate was then coated from the substrate side with an illuminance of 2.5 mW / cm. 2 , cumulative light intensity 2000 mJ / cm 2 The coating layer was photocured to form a primary cured layer, thereby obtaining a primary cured sheet. This primary cured sheet was left to stand at room temperature for 5 hours, then heated at 130°C for 3 minutes, and then left in an atmosphere at 50°C for 3 days to obtain a pressure-sensitive adhesive sheet. The coatability of the obtained pressure-sensitive adhesive sheet was evaluated. The results are shown in Table 1.
[0091] [Example 2] A pressure-sensitive adhesive sheet was obtained in the same manner as in Example 1, except that the standing time of the primary cured sheet was changed to 8 hours. The coatability of the obtained pressure-sensitive adhesive sheet was evaluated. The results are shown in Table 1.
[0092] [Example 3] A pressure-sensitive adhesive containing 100 parts by weight of polyester resin A-1, 5 parts by weight of composition B-1 containing acrylic resin, 0.01 parts by weight of dipentaerythritol hexaacrylate (DPHA), 12 parts by weight of diisocyanate (trade name "Duranate D101", manufactured by Asahi Kasei) as a crosslinking agent, 8 parts by weight of polyisocyanate (trade name "Coronate HX", manufactured by Tosoh), and 0.1 parts by weight of titanium tetraacetylacetonate as a catalyst was applied to the release-treated surface of a substrate (silicone release liner, manufactured by Mitsubishi Chemical Corporation, trade name "MRF38") to a thickness of 20 μm, and a cover release film was attached to the surface of the coating layer to obtain a laminate. This laminate was then applied from the substrate side with an illuminance of 2.5 mW / cm 2 , cumulative light intensity 2000 mJ / cm 2The adhesive layer was photocured to form a primary cured layer, and a primary cured sheet was obtained. After leaving this primary cured sheet at room temperature for 5 hours, the cover release film was peeled off, and the sheet was heated at 130°C for 1 minute and then left in an atmosphere at 50°C for 3 days to produce a pressure-sensitive adhesive sheet.
[0093] [Example 4] A pressure-sensitive adhesive sheet was obtained in the same manner as in Example 3, except that the standing time of the primary cured sheet was changed to 8 hours. The coatability of the obtained pressure-sensitive adhesive sheet was evaluated. The results are shown in Table 1.
[0094] Comparative Example 1 A pressure-sensitive adhesive composition containing 100 parts by weight of polyester resin A-1, 12 parts by weight of a diisocyanate (trade name "Duranate D101", manufactured by Asahi Kasei) as a crosslinking agent, 8 parts by weight of a polyisocyanate (trade name "Coronate HX", manufactured by Tosoh), and 0.1 parts by weight of titanium tetraacetylacetonate as a catalyst was applied to the release-treated surface of a release-treated polyethylene terephthalate (PET) film so that the thickness after drying would be 20 μm. The composition was heated at 130° C. for 1 minute and then left in an atmosphere at 50° C. for 3 days to obtain a pressure-sensitive adhesive sheet. The coatability of the obtained pressure-sensitive adhesive sheet was evaluated. The results are shown in Table 1.
[0095]
[0096] 10 Pressure-sensitive adhesive layer 20 Substrate 100 Pressure-sensitive adhesive sheet
Claims
1. A method for producing a pressure-sensitive adhesive sheet, comprising: a coating step of coating a substrate with a polyester-based pressure-sensitive adhesive to form a coating layer; a primary curing step of curing the coating layer with active energy rays to form a primary cured layer; and a secondary curing step of further curing the primary cured layer by heating after the primary curing step, wherein the polyester-based pressure-sensitive adhesive comprises a polyester-based resin, a crosslinking agent, an acrylic resin composition, and a photoinitiator, and the acrylic resin composition comprises an acrylic resin and a monomer component that constitutes the acrylic resin.
2. The method for producing an adhesive sheet according to claim 1, wherein the polyester-based adhesive further contains a polyfunctional acrylic monomer.
3. The method for producing an adhesive sheet according to claim 1, wherein the polyester-based adhesive is substantially free of organic solvents.
4. The method for producing an adhesive sheet according to claim 1, wherein the content of the photoreaction initiator is 0.001 parts by weight or more per 100 parts by weight of the polyester resin.
5. The method for producing an adhesive sheet according to claim 1, wherein the polyester-based adhesive further contains a crosslinking catalyst.
6. The method for producing a pressure-sensitive adhesive sheet according to claim 1, wherein the heating temperature in the secondary curing step is 90°C to 150°C.
Citation Information
Patent Citations
Method for bonding optical disc substrate
JP1993194928A
Double-sided adhesive tape
JP2014169420A
Pressure-sensitive adhesive and adhesive film
JP2019006925A
Adhesive sheet, display body and method for manufacturing display body
JP2019044024A
Polyester adhesive composition
WO2011081163A1
Cited By
Pressure-sensitive adhesive and method for producing same
WO2026115112A1