Substrate for liquid filter, and liquid filter
The development of a microporous polyolefin membrane with specific pore size and crystallinity characteristics addresses the challenge of filtering small particles and removing residual metals, enhancing the efficiency of liquid filters in semiconductor processes.
Patent Information
- Application Number
- PCT/JP2024/009380
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-11
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional liquid filters with microporous polyolefin membranes face challenges in achieving both a dense filter medium for removing small foreign matter and efficiently removing residual metals during cleaning, as densification of the membrane reduces cleaning efficiency and metal elution.
A microporous polyolefin membrane with a pore diameter of 1 nm to 35 nm, crystallinity of 45% or more, and specific structural and molecular weight characteristics, allowing for effective filtration and easy removal of residual metals during washing.
The solution enables efficient filtration of microparticles and easy removal of residual metals, addressing the limitations of conventional filters by maintaining filtration efficiency while ensuring metal elution during cleaning.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Liquid filter substrate and liquid filter
[0001] The present disclosure relates to a substrate for a liquid filter and a liquid filter.
[0002] Liquid compositions used in semiconductor lithography processes are filtered through a liquid filter before use to remove minute foreign matter from the liquid composition. The liquid filter contains a filter medium such as a pleated dense porous membrane or a bundle of hollow fibers. Polyolefin microporous membranes have been known as porous membranes used in liquid filter media. Patent Documents 1 to 7 disclose liquid filter substrates made of small-pore polyolefin microporous membranes. Polyolefins do not contain halogen elements, and therefore liquid filters using polyolefin microporous membranes as filter media are advantageous in that they have fewer restrictions on disposal after use and have a smaller environmental impact.
[0003] International Publication No. 2014 / 181760 International Publication No. 2014 / 181761 International Publication No. 2014 / 181762 JP 2014-217800 A JP 2014-218563 A JP 2018-167198 A International Publication No. 2020 / 022321
[0004] In general, the filter material of a liquid filter is washed after production and before use. By washing the filter material, fine powders and airborne dust generated during the production of the liquid filter are removed from the filter material, preventing these foreign substances from being mixed into the liquid being treated by the liquid filter. In addition, when washing the filter material, trace amounts of metals contained in the filter material itself are eluted and removed. Polyolefin microporous membranes may contain metals (such as calcium and zinc, which are derived from polyolefin polymerization catalysts or post-polymerization additives (e.g., metal soaps)) introduced into the polyolefin, which is the raw material for production. These metals are eluted and removed from the polyolefin microporous membrane when the filter material is washed. Metals contained in the filter material may elute into the liquid composition used in the lithography process when filtering the liquid composition, which may reduce the production yield of semiconductors. Therefore, it is desirable to remove them from the filter material before use.
[0005] However, with the miniaturization and densification of semiconductor wiring patterns, the need to remove even the smallest foreign matter (for example, microparticles with a particle size of a few nm) from the liquid composition used in lithography process is increasing.Therefore, liquid filters with denser filter media are required.However, the denser the filter media, the lower the cleaning efficiency of the filter media tends to be.As for polyolefin microporous membrane, the smaller its pore size, the lower the efficiency of the metal contained in the polyolefin microporous membrane being dissolved and removed when cleaning the filter media.
[0006] Furthermore, the densification of polyolefin microporous membrane also makes the elution and removal of metal difficult due to the following mechanism.Generally, the densification of polyolefin microporous membrane is realized by using ultra-high molecular weight polyolefin as raw material.Therefore, as a way to make polyolefin microporous membrane more dense, it is considered to increase the blending ratio of ultra-high molecular weight polyolefin, in other words, to reduce the blending ratio of high density polyolefin.However, in this case, the crystalline proportion of polyolefin in polyolefin microporous membrane decreases, and the amorphous proportion increases.The metal contained in raw material polyolefin is likely to remain in the amorphous of polyolefin, and the metal in the amorphous interior is difficult to eluate when cleaning filter material.
[0007] For the above reasons, it has been difficult to simultaneously densify the polyolefin microporous membrane and remove the residual metal.
[0008] The present disclosure has been made under the above circumstances, and an object of the present disclosure is to provide a substrate for a liquid filter that has a relatively small pore size but from which residual metals can be easily removed by washing.
[0009] Specific means for solving the above problems include the following aspects. <1> A substrate for liquid filters, comprising a polyolefin microporous membrane having a pore size of 1 nm to 35 nm and a polyolefin crystallinity of 45% or more. <2> The substrate for liquid filters according to <1>, wherein the polyolefin microporous membrane has a thickness of 3 μm to 20 μm. <3> The substrate for liquid filters according to <1> or <2>, wherein the polyolefin microporous membrane has a porosity of 35% to 70%. <4> The polyolefin microporous membrane has a water flow rate of 0.003 L / min / ft 2 / psi ~ 0.180L / min / ft 2 / psi. <5> The substrate for liquid filters according to any one of <1> to <4>, wherein the weight-average molecular weight of all polyolefins constituting the polyolefin microporous membrane is 800,000 or more. <6> The substrate for liquid filters according to any one of <1> to <5>, wherein the polyolefin microporous membrane is a polyethylene microporous membrane. <7> A liquid filter comprising the substrate for liquid filters according to any one of <1> to <6>.
[0010] According to the present disclosure, a substrate for a liquid filter is provided that has a relatively small pore size but is easy to wash to remove residual metals.
[0011]
[0023] The following describes embodiments of the present disclosure. These descriptions and examples are intended to illustrate the embodiments and are not intended to limit the scope of the embodiments.
[0012] In the present disclosure, a numerical range indicated using "to" indicates a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively. In the numerical ranges described in stages in the present disclosure, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. Furthermore, in the numerical ranges described in the present disclosure, the upper or lower limit value of that numerical range may be replaced with a value shown in an example.
[0013] In the present disclosure, the term "step" includes not only an independent step but also a step that cannot be clearly distinguished from other steps as long as the purpose of the step is achieved.
[0014] In the present disclosure, when referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the total amount of the multiple substances present in the composition is referred to unless otherwise specified. In the present disclosure, multiple types of particles corresponding to each component may be included. If the composition contains multiple types of particles corresponding to each component, the particle size of each component refers to the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified.
[0015] In this disclosure, MD (Machine Direction) refers to the longitudinal direction of a polyolefin microporous membrane produced in a continuous shape, and TD (Transverse Direction) refers to the plane direction of the polyolefin microporous membrane perpendicular to the MD. In this disclosure, TD is also referred to as the "width direction."
[0016] In the present disclosure, when the stacking relationship of each layer constituting a liquid filter or a liquid filter substrate is expressed as "upper" and "lower," the layer closer to the polyolefin microporous membrane is referred to as "lower," and the layer farther from the polyolefin microporous membrane is referred to as "upper."
[0017] In the present disclosure, the volume of a microporous membrane or porous layer excluding pores is referred to as the "solids volume."
[0018] <Liquid filter substrate> The liquid filter substrate of the present disclosure has a polyolefin microporous membrane. The liquid filter substrate of the present disclosure may be a substrate consisting of only a polyolefin microporous membrane, or a substrate in which a polyolefin microporous membrane is laminated with another porous membrane or porous layer. The liquid filter substrate of the present disclosure may have one polyolefin microporous membrane, or two or more polyolefin microporous membranes (i.e., two or more polyolefin microporous membranes may be stacked).
[0019] An example of an embodiment of the substrate for liquid filters of the present disclosure is a substrate consisting of only a polyolefin microporous membrane. An example of an embodiment of the substrate for liquid filters of the present disclosure is a substrate with a single-layer structure consisting of only one polyolefin microporous membrane.
[0020] The polyolefin microporous membrane in the liquid filter substrate of the present disclosure has a pore size of 1 nm to 35 nm and a polyolefin crystallinity of 45% or more. The pore size of the polyolefin microporous membrane in the liquid filter substrate of the present disclosure is 1 nm to 35 nm, allowing for the filtration of fine particles (e.g., particles with a particle size of 5 nm) contained in the liquid to be treated. The polyolefin microporous membrane in the liquid filter substrate of the present disclosure has a crystallinity of 45% or more, allowing for easy removal of residual metals by washing, even if they are present.
[0021] The metal contained in the raw polyolefin tends to remain in the amorphous polyolefin in the polyolefin microporous membrane, and the metal in the amorphous interior is not easily eluted when the filter material is washed.If the crystallinity of the polyolefin constituting the polyolefin microporous membrane is 45% or more, even if the metal is contained in the polyolefin microporous membrane, it is easy to remove it by washing.
[0022] The polyolefin microporous membrane contained in the liquid filter substrate of the present disclosure will be described in detail below.
[0023] [Polyolefin microporous membrane] A polyolefin microporous membrane refers to a membrane in which fibril-like polyolefin forms a three-dimensional network structure, has numerous micropores inside, and has a structure in which the micropores are connected, allowing gas or liquid to pass from one side to the other.
[0024] In the polyolefin microporous membrane, the polyolefin preferably accounts for 90% by mass or more of the polyolefin microporous membrane, more preferably 95% by mass or more, and even more preferably 99% by mass or more. The polyolefin microporous membrane may contain an organic filler, an inorganic filler, a surfactant, etc., within a range that does not affect the effects of the present disclosure.
[0025] The polyolefin microporous membrane may be hydrophobic or hydrophilic. Since polyolefin is a hydrophobic resin, the polyolefin microporous membrane itself is hydrophobic. The polyolefin microporous membrane may be a hydrophobic polyolefin microporous membrane that has not been subjected to a hydrophilization treatment, or a polyolefin microporous membrane that has been rendered hydrophilic by a hydrophilization treatment.
[0026] Examples of treatment methods for hydrophilizing a polyolefin microporous membrane include physical hydrophilization treatments (plasma treatment, corona discharge treatment, ultraviolet irradiation, electron beam irradiation, etc.), coating treatments with surfactants or hydrophilic materials (cellulose, polyvinyl alcohol, etc.), and graft polymerization of hydrophilic monomers.
[0027] [Pore size] The pore size of the polyolefin microporous membrane is 1 nm to 35 nm. When the pore size of the polyolefin microporous membrane is 1 nm or more, sufficient liquid permeability can be obtained. From this viewpoint, the pore size of the polyolefin microporous membrane is preferably 5 nm or more, more preferably 10 nm or more, even more preferably 11 nm or more, and particularly preferably 13 nm or more. When the pore size of the polyolefin microporous membrane is 35 nm or less, fine particles (e.g., particles with a particle size of 5 nm) contained in the liquid to be treated can be filtered out. From this viewpoint, the pore size of the polyolefin microporous membrane is preferably 33 nm or less, more preferably 32 nm or less, even more preferably 25 nm or less, and particularly preferably 22 nm or less.
[0028] The pore size of a polyolefin microporous membrane is the flow pore size measured by the half-dry method specified in ASTM E1294-89. The flow pore size is measured using a perm porometer (PMI, Capillary Flow Porometer, Model: CFP-1500A) and a fluorine-based inert liquid (product name: Fluorinert, surface tension 16.0 dyn / cm) as an immersion liquid. The measurement temperature is 25°C, and the measurement pressure is varied in the range of 0 psi to 500 psi. The flow pore size is measured at a total of five points along the TD of the polyolefin microporous membrane: the center, two points 50 mm apart from the center toward both ends, and two points 100 mm apart from the center toward both ends, and the average of these measurements is defined as the pore size of the polyolefin microporous membrane.
[0029] [Crystallization degree of polyolefin] The crystallinity of the polyolefin constituting the polyolefin microporous membrane is 45% or more, preferably 46% or more, more preferably 47% or more, even more preferably 48% or more, and particularly preferably 49% or more, from the viewpoint of facilitating removal of residual metals by washing. The crystallinity of the polyolefin constituting the polyolefin microporous membrane is preferably 65% or less, more preferably 60% or less, even more preferably 58% or less, and particularly preferably 57% or less, from the viewpoint of densifying the polyolefin microporous membrane. When the polyolefin microporous membrane is a polyethylene microporous membrane, the crystallinity of the polyethylene is also preferably within the above range.
[0030] The crystallinity of polyolefins is determined by wide-angle X-ray diffraction (WAXD). A sample of 10 mm MD x 3 mm TD was cut from the center of the polyolefin microporous membrane, and the MD and TD were aligned and laminated to a thickness of 1 mm. The sample was fixed in the sample holder of a 2D-WAXD device (model number: NANO-Viewer, Rigaku Corporation). The MD of the sample was fixed in the meridional direction so that X-rays were incident perpendicular to the surface of the polyolefin microporous membrane. Transmission measurements were performed under the following conditions: X-ray generator: Ultrax18 Tube voltage / current: 45 kV / 60 mA Target: CuKα (λ=0.1542 nm) Camera length: 95 mm Measurement time: 10 minutes Measurement temperature: Room temperature Detector: Imaging plate The two-dimensional data obtained with the imaging plate is converted into a 2θ profile, and peak fitting is performed using a Gaussian function / Lorentzian function = 50 / 50 in the range of 2θ = 8° to 33°. The integrated intensity of each peak is calculated, and the crystalline integrated intensity Ic, which is the sum of the peak intensities of the crystalline components, and the amorphous integrated intensity Ia, which is the sum of the peak intensities of the amorphous components, are calculated. The crystallinity Xc is calculated using the following formula: Xc (%) = Ic ÷ (Ic + Ia) × 100
[0031] [Thickness] From the viewpoint of obtaining mechanical strength and durability, the thickness of the polyolefin microporous membrane is preferably 3 μm or more, more preferably 4 μm or more, even more preferably 5 μm or more, and particularly preferably 6 μm or more. From the viewpoint of obtaining sufficient liquid permeability, relatively low filtration pressure, the ability to increase the filtration area by pleating or the like, and ease of processing to increase the filtration area, the thickness of the polyolefin microporous membrane is preferably 20 μm or less, more preferably 18 μm or less, even more preferably 16 μm or less, even more preferably 15 μm or less, and particularly preferably 14 μm or less.
[0032] The thickness of the polyolefin microporous membrane is determined by measuring 10 points with a contact thickness meter and averaging the measurements. The measurement points are set at 10 equally spaced points along the TD from near one end to near the other end.
[0033] [Porosity] The porosity of the polyolefin microporous membrane is preferably 35% or more, more preferably 38% or more, even more preferably 40% or more, and particularly preferably 42% or more, from the viewpoints of obtaining sufficient liquid permeability, relatively low filtration pressure, etc. The porosity of the polyolefin microporous membrane is preferably 70% or less, more preferably 66% or less, even more preferably 60% or less, even more preferably 57% or less, and particularly preferably 55% or less, from the viewpoints of obtaining mechanical strength and durability.
[0034] The porosity ε (%) of a polyolefin microporous membrane is calculated by the following formula: ε (%) = {1 - Ws / (ds·t)} × 100, where Ws is the basis weight (g / m) of the polyolefin microporous membrane. 2 ds: True density (g / cm) of the polyolefin microporous membrane. The polyolefin microporous membrane is cut into pieces measuring 10 cm in MD x 10 cm in TD from three locations, namely, the center and both end portions, and the mass is measured and divided by the area. The average value of the TD center and both end portions is calculated and designated as Ws. ds: True density (g / cm) of the polyolefin microporous membrane. 3 t: thickness of polyolefin microporous membrane (μm): determined as above.
[0035] [Water Flow Rate] The water flow rate of the polyolefin microporous membrane is set to 0.003 L / min / ft from the viewpoint of obtaining sufficient liquid permeability for a long period of time. 2 / psi or more is preferred, and 0.004 L / min / ft 2 / psi or more is more preferred, and 0.005 L / min / ft 2 / psi or more is more preferred, and 0.007 L / min / ft 2 From the viewpoint of obtaining a collection performance for fine particles (e.g., particles with a particle size of 5 nm), the water flow rate of the polyolefin microporous membrane is preferably 0.180 L / min / ft 2 / psi or less is preferred, and 0.170 L / min / ft 2 / psi or less is more preferred, and 0.150 L / min / ft 2 / psi or less is more preferred, and 0.140 L / min / ft 2 / psi or less is particularly preferred.
[0036] The water flow rate of a polyolefin microporous membrane is determined by the following measurement method. A polyolefin microporous membrane is cut into 40 mm x 40 mm squares from three locations, namely the center and both end portions of the polyolefin microporous membrane, and the squares are immersed in ethanol and dried at room temperature. The polyolefin microporous membrane is placed in a 37 mm diameter liquid permeation cell (liquid permeation area 10.75 cm). 2 ), and 100 ml of pure water is passed through at a differential pressure of 90 kPa under a temperature atmosphere of 24°C, and the time Tl (min) required for the entire amount of pure water to pass through is measured. The volume V (100 ml) of pure water, the time Tl (min), and the liquid permeation area S (10.75 cm 2 ) and the water flow rate Vs (unit time (min) under 1 psi differential pressure) × unit area (ft 2 ) and the unit is L / min / ft 2 / psi). Furthermore, calculate the average value near the center and both ends of the TD. Vs = (V / 1000) / Tl / (S / 929.03) / (90 / 6.895)
[0037] [Heat shrinkage rate] From the viewpoint of heat resistance, the heat shrinkage rate of the polyolefin microporous membrane at a temperature of 105°C is preferably 45% or less, more preferably 40% or less, and even more preferably 30% or less in MD. From the viewpoint of heat resistance, the heat shrinkage rate of the polyolefin microporous membrane at a temperature of 105°C is preferably 20% or less, more preferably 15% or less, and even more preferably 10% or less in TD.
[0038] The heat shrinkage of a polyolefin microporous membrane is determined by the following measurement method. A polyolefin microporous membrane is cut into a sample measuring 10 cm in MD x 10 cm in TD from three locations: the center and both ends. The sample is placed in an oven maintained at a temperature of 105°C for 30 minutes. The sample is removed from the oven, and the MD and TD lengths of the sample are measured. The heat shrinkage (%) in each of the MD and TD directions is calculated as follows: (length before heat treatment - length after heat treatment) ÷ length before heat treatment × 100). Furthermore, the average values for the center and both ends in TD are calculated.
[0039] [Polyolefin] Examples of polyolefins constituting the polyolefin microporous membrane include homopolymers (i.e., polyethylene, polypropylene, polybutylene, polymethylpentene, etc.) or copolymers of ethylene, propylene, butylene, methylpentene, etc., and mixtures thereof.
[0040] The polyolefin microporous membrane is preferably a microporous membrane formed using two or more polyolefins that differ from each other in at least one of the type of monomer, degree of polymerization, degree of branching, crystallinity, stretchability, and molecular orientation. By using two or more polyolefins, a network structure is easily formed in the polyolefin microporous membrane by fibrillation during stretching.
[0041] The weight-average molecular weight of all the polyolefins constituting the polyolefin microporous membrane is preferably 800,000 or more, more preferably 850,000 or more, even more preferably 900,000 or more, even more preferably 950,000 or more, and particularly preferably 970,000 or more, from the viewpoint of densifying the polyolefin microporous membrane. The weight-average molecular weight of all the polyolefins constituting the polyolefin microporous membrane is preferably 3,500,000 or less, more preferably 3,200,000 or less, even more preferably 3,100,000 or less, and particularly preferably 3,000,000 or less, from the viewpoint of facilitating uniform melting during melt-kneading.
[0042] The weight average molecular weight of the entire polyolefin constituting the polyolefin microporous membrane is determined by heating and dissolving the polyolefin microporous membrane in o-dichlorobenzene and measuring the molecular weight by gel permeation chromatography (system: Alliance GPC 2000 manufactured by Waters Corporation, columns: GMH6-HT and GMH6-HTL) at a column temperature of 135°C and a flow rate of 1.0 mL / min. Monodisperse polystyrene (Tosoh Corporation) is used for molecular weight calibration.
[0043] The polyolefin constituting the polyolefin microporous membrane is preferably polyethylene. That is, the polyolefin microporous membrane is preferably a polyethylene microporous membrane. In the present disclosure, a polyethylene microporous membrane refers to a microporous membrane in which polyethylene is the resin that accounts for the largest proportion by mass of all resins.
[0044] In the polyethylene microporous membrane, polyethylene preferably accounts for 90% by mass or more of the polyethylene microporous membrane, more preferably 95% by mass or more, and even more preferably 99% by mass or more. The polyethylene microporous membrane may contain an organic filler, an inorganic filler, a surfactant, etc., as long as the effects of the present disclosure are not affected.
[0045] The polyethylene microporous membrane is preferably a microporous membrane formed using two or more polyethylenes that differ from each other in at least one of degree of polymerization, degree of branching, crystallinity, stretchability, and molecular orientation. Using two or more polyethylenes facilitates the formation of a network structure in the polyethylene microporous membrane by fibrillation during stretching.
[0046] Examples of polyethylene that can be used to form the microporous polyethylene film include ultra-high molecular weight polyethylene, high-density polyethylene, and a mixture of ultra-high molecular weight polyethylene and high-density polyethylene.
[0047] From the viewpoint of densifying the polyethylene microporous membrane, the polyethylene microporous membrane preferably contains ultra-high molecular weight polyethylene having a weight-average molecular weight of 3,000,000 to 6,000,000.The polyethylene microporous membrane preferably contains 50% to 95% by mass, more preferably 60% to 90% by mass, and even more preferably 70% to 85% by mass of ultra-high molecular weight polyethylene having a weight-average molecular weight of 3,000,000 to 6,000,000.
[0048] The polyethylene microporous membrane is made of ultra-high molecular weight polyethylene with a weight average molecular weight of 3 million to 6 million, and polyethylene with a weight average molecular weight of 200,000 to 800,000 and a density of 0.92 g / cm 3 ~0.98g / cm 3 The mass ratio of the two polyethylenes in the polyethylene microporous membrane (ultra-high molecular weight polyethylene:high-density polyethylene) is preferably 50:50 to 95:5, more preferably 60:40 to 90:10, and even more preferably 70:30 to 85:15, from the viewpoint of increasing the crystallinity of the polyethylene and producing a microporous membrane with a small pore size.
[0049] The weight average molecular weight of the entire polyethylene constituting the polyethylene microporous membrane is preferably 800,000 or more, more preferably 850,000 or more, even more preferably 900,000 or more, still more preferably 950,000 or more, and particularly preferably 970,000 or more, from the viewpoint of densifying the polyethylene microporous membrane. The weight average molecular weight of the entire polyethylene constituting the polyethylene microporous membrane is preferably 3,500,000 or less, more preferably 3,200,000 or less, even more preferably 3,100,000 or less, and particularly preferably 3,000,000 or less, from the viewpoint of facilitating uniform melting during melt-kneading.
[0050] The calcium content contained in the polyolefin constituting the polyolefin microporous membrane varies depending on the raw material polyolefin, but is preferably within the following ranges, for example. In one embodiment, the calcium content contained in the polyolefin is preferably 50 ppm or less, more preferably 38 ppm or less, even more preferably 35 ppm or less, and particularly preferably 34 ppm or less. In one embodiment, the calcium content contained in the polyolefin is preferably 1000 ppb or less, more preferably 500 ppb or less, even more preferably 400 ppb or less, and particularly preferably 300 ppb or less. The calcium content contained in the polyolefin is, for example, 0 ppb or more, 10 ppb or more, 20 ppb or more, 50 ppb or more, or 100 ppb or more. Methods for adjusting the calcium content in the polyolefin include adjusting the amount of metal soap (such as calcium stearate) added to the polyolefin after polymerization, acid washing the polyolefin, and removing the polymerization catalyst remaining in the polyolefin by a deashing process.
[0051] The calcium content of the polyolefin is determined by adding ultra-high purity nitric acid to the polyolefin, decomposing it with microwaves, and using this as a sample to quantify it using ICP-MS (inductively coupled plasma mass spectrometry, instrument name: Agilent 7500cs, Agilent Technologies, Inc.).
[0052] [Method for Producing Microporous Polyolefin Membrane] The microporous polyolefin membrane can be produced, for example, by a method including the following steps (1) to (6).
[0053] Step (1): A step of preparing a polyolefin solution containing a polyolefin and a solvent. Step (2): A step of melt-kneading the polyolefin solution, extruding the melt-kneaded mixture through a die, and cooling and solidifying the extrudate to obtain a gel-like molded product. Step (3): A step of squeezing the solvent out of the gel-like molded product. Step (4): A step of stretching the gel-like molded product in at least one direction to obtain a polyolefin microporous membrane. Step (5): A step of washing the polyolefin microporous membrane to remove the solvent. Step (6): A step of annealing the polyolefin microporous membrane.
[0054] The crystallinity of the polyolefin constituting the polyolefin microporous membrane can be adjusted by controlling the conditions of steps (1), (2), and (4). Furthermore, the thickness, pore size, porosity, water flow rate, etc. of the polyolefin microporous membrane can be adjusted by controlling the conditions of steps (1) to (6).
[0055] -Step (1)- Step (1) is a step of preparing a polyolefin solution containing a polyolefin and a solvent.
[0056] The polyolefin used in step (1) may be one type or two or more types. The polyolefin preferably contains polyethylene, and is preferably a polyethylene having an ultra-high molecular weight of 3,000,000 to 6,000,000 and a high molecular weight polyethylene having a weight-average molecular weight of 200,000 to 800,000 and a density of 0.92 g / cm. 3 ~0.98g / cm 3 and a high density polyethylene.
[0057] Polyolefins are generally traded in the form of granular pellets or powder. When polyolefin powder is used in step (1), the particle size of the powder is preferably 1 μm to 1000 μm, more preferably 5 μm to 500 μm, and even more preferably 10 μm to 300 μm, from the viewpoint of uniformly melt-kneading the polyolefin in step (2) and increasing the crystallinity of the polyolefin. The particle size mentioned above is the median diameter (d50) of the volume-based particle size distribution. The volume-based particle size distribution is determined by dry measurement using a laser diffraction particle size distribution analyzer (instrument name: Mastersizer 2000, Malvern Instruments).
[0058] The solvent used in step (1) is not limited as long as it can swell or dissolve the polyolefin. Solvents are broadly classified into non-volatile solvents having a boiling point of 210°C or higher at atmospheric pressure and volatile solvents having a boiling point of less than 210°C at atmospheric pressure.
[0059] Examples of non-volatile solvents include liquid paraffin, paraffin oil, mineral oil, and castor oil. The non-volatile solvents may be used alone or in combination of two or more. Liquid paraffin is preferred as the non-volatile solvent.
[0060] Examples of volatile solvents include tetralin, ethylene glycol, decalin (also known as decahydronaphthalene), toluene, xylene, diethyltriamine, ethylenediamine, dimethyl sulfoxide, and hexane. One type of volatile solvent may be used alone, or two or more types may be used in combination. Decalin or xylene is preferred as the volatile solvent.
[0061] The solvent used in step (1) is preferably a mixed solvent of a nonvolatile solvent and a volatile solvent, more preferably a mixed solvent of liquid paraffin and decalin or xylene, and even more preferably a mixed solvent of liquid paraffin and decalin. The mixing ratio of the nonvolatile solvent to the volatile solvent (mass ratio, nonvolatile solvent:volatile solvent) is preferably 99:1 to 60:40.
[0062] When two or more polyolefins are used, the order in which the polyolefins and the solvent are mixed is not limited. For example, either of the following forms (a) and (b) may be used.
[0063] Mode (a): Two or more polyolefins are mixed one by one in a solvent. Two or more solvents may be mixed in advance to prepare a mixed solvent, and the polyolefins may be mixed one by one in the mixed solvent.
[0064] Mode (b): Two or more polyolefins are mixed to prepare a polyolefin composition, and the polyolefin composition is then mixed with a solvent. Alternatively, two or more solvents may be mixed in advance to prepare a mixed solvent, and the mixed solvent and the polyolefin composition may then be mixed.
[0065] From the viewpoint of imparting a good balance between mechanical strength, liquid permeability, and fine particle collection performance to the polyolefin microporous membrane, the polyolefin concentration of the polyolefin solution is preferably 10% by mass to 40% by mass, more preferably 15% by mass to 35% by mass, and even more preferably 20% by mass to 30% by mass. When the polyolefin concentration of the polyolefin solution is 10% by mass or more, the mechanical strength of the polyolefin microporous membrane is ensured. When the polyolefin concentration of the polyolefin solution is 40% by mass or less, pores are likely to form in the polyolefin microporous membrane.
[0066] Step (2) is a step of melt-kneading the polyolefin solution, extruding the melt-kneaded mixture through a die, and cooling and solidifying the extrudate to obtain a gel-like molded product. The gel-like molded product is preferably formed into a sheet.
[0067] The melt-kneading of the polyolefin solution is preferably carried out using a kneading extruder. A kneading extruder is a device that applies pressure and heat to a material to be treated while continuously conveying the material. The structure of a kneading extruder is generally broadly divided into a material inlet, a barrel, and a die, from upstream to downstream. A screw is provided inside the barrel. A heater that heats the inside of the barrel is provided around the barrel. The screw may be a single-screw type or a twin-screw type, with the twin-screw type being preferred.
[0068] From the viewpoint of sufficiently melting the polyolefin, the temperature of the polyolefin solution in the most downstream region inside the barrel is preferably MP+30°C to MP+150°C, more preferably MP+40°C to MP+140°C, and even more preferably MP+50°C to MP+130°C, where MP°C is the melting point of the polyolefin (when two or more polyolefins are used, MP°C is the highest melting point among those polyolefins).
[0069] The time required for the material to pass through the barrel is preferably 1 minute to 10 minutes, more preferably 1 minute 30 seconds to 8 minutes, and even more preferably 2 minutes to 7 minutes. The time required for the material to pass through the barrel can be controlled by the rotation speed of the screw.
[0070] From the viewpoint of improving the film formability of the polyolefin microporous membrane, the temperature of the molten kneaded material in the die is preferably MP+30°C to MP+120°C, more preferably MP+40°C to MP+110°C, and even more preferably MP+50°C to MP+100°C, where MP°C is the melting point of the polyolefin (when two or more polyolefins are used, the highest melting point among those polyolefins is defined as MP°C).
[0071] Methods for cooling the extrudates include, for example, immersing the extrudates in water or an organic solvent, or contacting the extrudates with a cooled metal roll. The cooling temperature is preferably 10° C. to 40° C. When immersing the extrudates in water, it is preferable to create a water flow on the surface of the water bath to prevent the solvent released from the extrudates from adhering to the extrudates.
[0072] -Step (3)- Step (3) is a step of squeezing the solvent out of the gel-like molded product. Step (3) is preferably achieved by applying pressure to the gel-like molded product. Methods for applying pressure to the gel-like molded product include, for example, conveying the gel-like molded product while pressing it against a roller or a belt, or passing the gel-like molded product between a pair of rollers. The pressure to which the gel-like molded product is subjected is preferably 0.01 MPa to 0.5 MPa, more preferably 0.05 MPa to 0.2 MPa. The surface temperature of the roller or belt is preferably 40°C to 100°C.
[0073] Between steps (2) and (3), it is preferable to heat-treat the gel-like molding for the purpose of volatilizing a part of the solvent from the gel-like molding. The temperature of the heat-treating is preferably 50°C to 100°C. The heat-treating may be performed once or twice or more times at different temperatures. The heat-treating time is preferably 5 minutes to 10 minutes per time. By performing the heat-treating in advance, it is possible to shorten the conveying path in step (3) and to make the conditions (pressure and / or temperature) of step (3) milder.
[0074] -Step (4)- Step (4) is a step of stretching the gel-like molding in at least one direction to obtain a microporous polyolefin membrane.
[0075] The stretching in step (4) is preferably biaxial stretching. The biaxial stretching may be either sequential biaxial stretching in which longitudinal stretching and transverse stretching are performed separately, or simultaneous biaxial stretching in which longitudinal stretching and transverse stretching are performed simultaneously. The biaxial stretching may be performed by stretching multiple times in the longitudinal direction and then stretching in the transverse direction, by stretching in the longitudinal direction and then stretching multiple times in the transverse direction, or by sequential biaxial stretching and then further stretching once or multiple times in the longitudinal and / or transverse directions.
[0076] The stretching ratio (the product of the longitudinal stretching ratio and the transverse stretching ratio) is preferably 40 to 200 times, more preferably 45 to 180 times, and even more preferably 50 to 150 times, from the viewpoint of imparting a good balance between liquid permeability and microparticle collection performance to the polyolefin microporous membrane, and from the viewpoint of increasing the crystallinity of the polyolefin constituting the polyolefin microporous membrane.
[0077] The stretching temperature is preferably 90°C to 130°C, more preferably 95°C to 125°C, and even more preferably 100°C to 120°C, from the viewpoint of increasing the crystallinity of the polyolefin constituting the microporous polyolefin membrane.
[0078] The heat setting temperature is preferably 100°C to 140°C, more preferably 105°C to 135°C, and even more preferably 110°C to 133°C, from the viewpoint of increasing the crystallinity of the polyolefin constituting the polyolefin microporous membrane.
[0079] Step (5) is a step of washing the polyolefin microporous membrane to remove the solvent. In step (5), the polyolefin microporous membrane is preferably washed with a solvent such as a halogenated hydrocarbon such as methylene chloride or a hydrocarbon such as hexane.
[0080] The cleaning of the polyolefin microporous membrane is preferably carried out by immersing the polyolefin microporous membrane in a bath containing a cleaning solvent. In this case, to enhance the cleaning effect, it is preferable to divide the bath into two or more tanks and increase the purity of the cleaning solvent in the downstream bath. This can be achieved by pouring the cleaning solvent into the most downstream bath and allowing it to flow upstream. When dividing the bath into two or more tanks, there may be two or three or more tanks. From the viewpoint of achieving a gentler gradient in the purity of the cleaning solvent in each tank, three or more tanks are preferred. The time required for the polyolefin microporous membrane to pass through all the baths is preferably 60 to 150 seconds, more preferably 70 to 120 seconds, and even more preferably 80 to 100 seconds.
[0081] After the polyolefin microporous membrane is removed from the bath containing the cleaning solvent, the cleaning solvent is preferably removed by drying at a temperature slightly above the boiling point of the cleaning solvent.
[0082] -Step (6)- Step (6) is a step of annealing the polyolefin microporous membrane. The annealing is carried out, for example, by transporting the polyolefin microporous membrane on rollers having a surface temperature of 100°C to 130°C or through a thermostatic bath having a temperature of 100°C to 130°C. During the annealing, it is preferable to fix the polyolefin microporous membrane in the width direction to suppress shrinkage of the polyolefin microporous membrane in the width direction.
[0083] Furthermore, the polyolefin microporous membrane may be subjected to a treatment to impart affinity to the liquid to be treated by the liquid filter.
[0084] <Liquid Filter> The liquid filter of the present disclosure is a device for removing microparticles from a liquid to be treated that contains or may contain the particles in a solid or gel form.
[0085] The liquid filter of the present disclosure includes the liquid filter substrate of the present disclosure as a filter medium. While the filter medium of a liquid filter is generally washed after manufacture and before use, the liquid filter substrate of the present disclosure allows for easy removal of residual metals by washing, even if the residual metals are present. Therefore, if the filter medium of the liquid filter of the present disclosure is washed before use, there is little concern about metals eluting into the liquid to be treated when filtering the liquid.
[0086] The liquid filter of the present disclosure includes, for example, a pleated liquid filter substrate and a cylindrical housing, with the pleated liquid filter substrate housed inside the housing. The liquid filter of the present disclosure is, for example, a cartridge that is detachable from a filtration device.
[0087] The liquid filter of the present disclosure is suitable for removing fine particles having a particle size of about several nanometers from a liquid to be treated. The liquid filter of the present disclosure can be used, for example, in the manufacturing process of semiconductors and displays.
[0088] The liquid filter substrate of the present disclosure will be described in more detail below with reference to examples. The materials, amounts used, ratios, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present disclosure. Therefore, the scope of the liquid filter substrate of the present disclosure should not be interpreted as being limited by the specific examples shown below.
[0089] In the following description, syntheses, treatments, manufacturing, etc. were carried out at room temperature (25° C.±3° C.) unless otherwise specified.
[0090] <Measurement methods and evaluation methods> In all of the Examples and Comparative Examples, a polyolefin microporous membrane with a width of 270 mm was produced by winding it around a winding core with an inner diameter of 3 inches. Samples cut to appropriate dimensions from the produced polyolefin microporous membrane were subjected to physical property measurement or performance evaluation. The methods for measuring physical properties and evaluating performance were as follows.
[0091] [Calcium Content of Polyolefin] 0.1 g of polyolefin was precisely weighed into a fluororesin container, and ultra-high purity nitric acid was added and decomposed using microwaves. The calcium (Ca) content was quantified in ppb order using ICP-MS (inductively coupled plasma mass spectrometry, Agilent 7500cs, Agilent Technologies, Inc.).
[0092] [Particle size of polyolefin powder] The volumetric particle size distribution of the polyolefin powder was determined by dry measurement using a laser diffraction particle size distribution analyzer (device name: Mastersizer 2000, Malvern Instruments), and the median diameter (d50) was taken as the particle size.
[0093] [Thickness of polyolefin microporous membrane] Using a contact-type thickness meter (Mitutoyo Corporation) and a cylindrical contact tip with a bottom diameter of 0.5 cm, the thickness (μm) of the polyolefin microporous membrane was measured at 10 points at 26 mm intervals along the TD, and the measured values were averaged. The measurement pressure of the contact tip was 0.1 N.
[0094] [Porosity of Polyolefin Microporous Membrane] The porosity (ε) of a polyolefin microporous membrane was calculated using the following formula: ε (%) = {1 - Ws / (ds·t)} × 100, where Ws is the basis weight (g / m) of the polyolefin microporous membrane. 2 ds: True density (g / cm) of the polyolefin microporous membrane. The polyolefin microporous membrane was cut into pieces measuring 10 cm in MD x 10 cm in TD from three locations, namely, the center and both end portions, and the mass was measured and divided by the area. Furthermore, the average value of the masses at the center and both end portions was calculated and designated as Ws. ds: True density (g / cm) of the polyolefin microporous membrane. 3 t: thickness of polyolefin microporous membrane (μm): determined by the measurement described above.
[0095] [Pore diameter of polyolefin microporous membrane] The flow pore diameter was measured at a total of five points along the TD of the polyolefin microporous membrane: the center, two points 50 mm away from the center toward both ends, and two points 100 mm away from the center toward both ends, and the measured values were averaged. The flow pore diameter was measured as follows. Using a perm porometer (PMI, Capillary Flow Porometer, Model: CFP-1500A) and a fluorine-based inert liquid (product name: Fluorinert, surface tension 16.0 dyn / cm) as the immersion liquid, the flow pore diameter was measured by the half-dry method specified in ASTM E1294-89. The measurement temperature was 25°C, and the measurement pressure was changed in the range of 0 psi to 500 psi, under the following conditions. Bubble point parameters: BUBLFLOW = 50, F / PT = 100, MINBPPRES = 0, ZEROTIME = 1, PULSEDELAY = 2 Wet parameters: V2INCR = 15, PREGINC = 0.9, MINEQTIME = 30, PRESSLEW = 30, FLOWSLEW = 30, EQITER = 50, AVEITER = 10, MAXPDIF = 1, MAXFDIF = 30 Dry parameters: V2INCR = 40, PREGINC = 2.4, MINEQTIME = 30, PRESSLEW = 30, FLOWSLEW = 30, EQITER = 40, AVEITER = 10, MAXPDIF = 1, MAXFDIF = 30
[0096] [Water flow rate of polyolefin microporous membrane] A polyolefin microporous membrane was cut into 40 mm x 40 mm squares from three locations, namely, the center and both end portions of the TD, and each square was immersed in ethanol and dried at room temperature. The polyolefin microporous membrane was then passed through a stainless steel liquid permeation cell with a diameter of 37 mm (liquid permeation area 10.75 cm). 2The polyolefin microporous membrane on the liquid permeation cell was wetted with a small amount (0.5 ml) of ethanol, and then 100 ml of pure water was passed through it at a temperature of 24°C and a differential pressure of 90 kPa. The time Tl (min) required for the entire amount of pure water to pass through was measured. The volume V (100 ml) of pure water, the time Tl (min), and the liquid permeation area S (10.75 cm 2 ) and the water flow rate Vs (unit time (min) under 1 psi differential pressure) × unit area (ft 2 ) and the unit is L / min / ft 2 / psi) was calculated, and the average value near the center and both ends of the TD was calculated. Vs = (V / 1000) / Tl / (S / 929.03) / (90 / 6.895)
[0097] [Weight-average molecular weight (Mw) of polyolefin] A polyolefin microporous membrane was dissolved in o-dichlorobenzene by heating, and the molecular weight was measured by gel permeation chromatography (system: Alliance GPC 2000 manufactured by Waters Corporation, columns: GMH6-HT and GMH6-HTL) at a column temperature of 135°C and a flow rate of 1.0 mL / min. Monodisperse polystyrene (Tosoh Corporation) was used to calibrate the molecular weight.
[0098] [Polyolefin Crystallinity] A polyolefin microporous membrane was cut from the center of the TD to a size of 10 mm in MD × 3 mm in TD, and laminated to a thickness of 1 mm with the MD and TD oriented in the same direction to prepare a sample. The sample was fixed in the sample holder of a 2D-WAXD device (model number: NANO-Viewer, Rigaku Corporation). The MD of the sample was fixed in the meridional direction so that X-rays were incident perpendicular to the surface of the polyolefin microporous membrane. Transmission measurements were performed under the following conditions. X-ray generator: Ultrax18; Tube voltage / current: 45 kV / 60 mA; Target: CuKα (λ=0.1542 nm); Camera length: 95 mm; Measurement time: 10 minutes; Measurement temperature: Room temperature; Detector: Imaging plate. The two-dimensional data obtained with the imaging plate was converted into a 2θ profile, and peak fitting was performed using a Gaussian function / Lorentzian function = 50 / 50 in the range of 2θ=8° to 33°. The integrated intensity of each peak was calculated, and the crystalline integrated intensity Ic, which is the sum of the peak intensities of the crystalline components, and the amorphous integrated intensity Ia, which is the sum of the peak intensities of the amorphous components, were calculated. The crystallinity Xc was calculated using the following formula: Xc (%) = Ic ÷ (Ic + Ia) × 100
[0099] [Collection Performance] Gold colloid with a particle size of 5 nm (Funakoshi Co., Ltd., particle size range: 4.5 to 6.0 nm) was dispersed in water to prepare a dispersion with a gold colloid concentration of 40 ppb. A polyolefin microporous membrane was cut into 50 mm x 50 mm squares from three locations, namely the center and both end portions of the TD, and each was immersed in ethanol and dried at room temperature. The polyolefin microporous membrane was then passed through a 37 mm diameter stainless steel liquid permeation cell (liquid permeation area: 10.75 cm). 2). The polyolefin microporous membrane on the liquid permeation cell was wetted with a small amount (0.5 ml) of ethanol, and then 200 ml of the gold colloid dispersion was passed through it at a differential pressure of 0.1 MPa. The metal concentration of the gold colloid dispersion after passing through the polyolefin microporous membrane was measured and quantified using ICP-OES (inductively coupled plasma optical emission spectroscopy, instrument name: Agilent-ICP-OES-5100, Agilent Technologies, Inc.). A calibration curve for quantification was created using standard gold colloid dispersions (five or more samples were prepared in the concentration range of 0 ppb to 100 ppb). The capture efficiency (%) = {(M1 - M2) ÷ M1 × 100} was calculated from the initial metal concentration M1 (i.e., 40 ppb) of the gold colloid dispersion and the metal concentration M2 of the gold colloid dispersion after passing through the polyolefin microporous membrane. Furthermore, the average values near the center and both ends of the TD were calculated and the average values were classified as follows: A: Average capture efficiency of 90% or more B: Average capture efficiency of less than 90%, 80% or more C: Average capture efficiency of less than 80%
[0100] [Metal elution] Adherents (fine powder generated during the production of the polyolefin microporous membrane, dust in the air, and the like that were not integrated with the polyolefin microporous membrane) were removed from both sides of the polyolefin microporous membrane. The polyolefin microporous membrane was cut into square pieces (10 cm x 10 cm, 40 pieces, total area 4000 cm). 2), which was used as a sample. The sample was placed in a fluororesin container, and 200 g of hydrochloric acid extract (a liquid containing 10 mass% hydrochloric acid in a mixed solution of water and isopropyl alcohol = 40:60 (mass ratio)) was poured into it, and the sample was immersed in the hydrochloric acid extract. After 24 hours, the sample was removed and dried. The dried sample was placed in another fluororesin container, and 200 g of propylene glycol monomethyl ether (PGME) was poured into it, and the sample was immersed in PGME. After 24 hours and 168 hours, the Ca and Zn concentrations in the PGME were quantified to the order of 0.1 ppb using ICP-OES (inductively coupled plasma optical emission spectroscopy, instrument name: Agilent-ICP-OES-5100, Agilent Technologies, Inc.). From the quantified Ca and Zn concentrations, the mass of PGME, and the sample area, the total amount of Ca and Zn eluted from the polyolefin microporous membrane (μg / m 2 The increase rate of the amount of elution (%) = {(total amount of elution after 168 hours - total amount of elution after 24 hours) / total amount of elution after 24 hours x 100} was calculated and classified as follows: A: The increase rate of the amount of elution is less than 5% B: The increase rate of the amount of elution is 5% or more but less than 10% C: The increase rate of the amount of elution is 10% or more
[0101] [TD Heat Shrinkage Rate] A polyolefin microporous membrane was cut into a size of 10 cm in MD x 10 cm in TD from a total of three locations: the center and near both ends. The sample was placed in an oven maintained at 105°C for 30 minutes. The sample was removed from the oven, and the TD length of the sample was measured. The TD heat shrinkage rate (%) = {(TD length before heat treatment - TD length after heat treatment) ÷ TD length before heat treatment × 100} was calculated. Furthermore, the average value of the TD center and near both ends was calculated and classified as follows: A: TD heat shrinkage rate is 10% or less B: TD heat shrinkage rate is more than 10% and 20% or less C: TD heat shrinkage rate is more than 20%
[0102] <Production of substrate for liquid filter> Hereinafter, "UHMWPE" means ultra-high molecular weight polyethylene having a weight average molecular weight of 3 million to 6 million, and "HDPE" means polyethylene having a weight average molecular weight of 200,000 to 800,000 and a density of 0.92 g / cm 3 ~0.98g / cm3 means high density polyethylene.
[0103] Example 1 - Step (1) - UHMWPE with a Mw of 4.6 million and a Ca content of 140 ppb: 22 parts by mass (UHMWPE powder particle size: 60 μm) HDPE with a Mw of 500,000 and a Ca content of 230 ppb: 5 parts by mass (HDPE powder particle size: 250 μm) Liquid paraffin: 72 parts by mass Decalin: 1 part by mass The above materials were prepared. Liquid paraffin and decalin were mixed to prepare a mixed solvent. The entire amount of UHMWPE was added to the mixed solvent and stirred and mixed. Next, the entire amount of HDPE was added and stirred and mixed. In this way, a polyethylene solution with a polyethylene concentration of 27% by mass was prepared. The Ca content in the mixture of UHMWPE and HDPE was 157 ppb.
[0104] -Step (2)- The polyethylene solution was charged into a twin-screw kneading extruder, and pressure and heat were applied to the polyethylene solution by operating it at a screw rotation speed of 200 rpm. The temperature inside the barrel of the twin-screw kneading extruder was adjusted so that the polyethylene solution temperature in the most downstream region was 200°C, and the polyethylene solution temperature at the die was adjusted so that it was 190°C. The polyethylene solution was extruded from the die in the form of a sheet, and the extrudate was conveyed to a water bath at a water temperature of 20°C and cooled to produce a base tape that was a gel-like sheet.
[0105] -Step (3)- The base tape was removed from the water bath, and then transported through a space at a temperature of 60°C for 10 minutes, and then transported through a space at a temperature of 95°C for 10 minutes to remove decalin from the base tape. Next, the base tape was transported on a roller having a surface temperature of 90°C while applying a pressure of 0.05 MPa to remove some of the liquid paraffin from the base tape.
[0106] -Step (4)- The base tape was stretched 7 times in MD at a temperature of 100°C (longitudinal stretching), and then stretched 25 times in TD at a temperature of 115°C (transverse stretching), followed immediately by heat setting at a temperature of 115°C to obtain a polyolefin microporous membrane.
[0107] -Step (5)- The polyolefin microporous membrane was continuously immersed in three separate methylene chloride baths (referred to as the first, second, and third tanks from the upstream side) for 30 seconds each to extract liquid paraffin from the polyolefin microporous membrane. Methylene chloride was poured into the third tank, and flowed from the third tank to the first tank to form a gradient in the purity of the methylene chloride (first tank < second tank < third tank). The polyolefin microporous membrane was removed from the methylene chloride bath and transported through a space at a temperature of 40°C to remove the methylene chloride from the polyolefin microporous membrane.
[0108] -Step (6)- The polyolefin microporous membrane was annealed by conveying it through a thermostatic bath at 110°C for 1 minute while keeping the TD length constant, then conveyed through a space at 60°C for 20 seconds, and then conveyed into a space at room temperature to cool.
[0109] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, with numerous micropores inside that were connected to each other, allowing gas or liquid to pass through from one side to the other. The properties of this polyethylene microporous membrane (liquid filter substrate of the present disclosure) are shown in Table 1.
[0110] Example 2 A polyethylene microporous membrane was produced in the same manner as in Example 1, except that step (4) was changed as follows.
[0111] -Step (4)- The base tape was stretched 6 times in MD at a temperature of 100°C (longitudinal stretching), then stretched 16 times in TD at a temperature of 110°C (transverse stretching), and then immediately heat-set at a temperature of 120°C to obtain a polyolefin microporous membrane.
[0112] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, with numerous micropores inside that were connected to each other, allowing gas or liquid to pass through from one side to the other. The properties of this polyethylene microporous membrane (liquid filter substrate of the present disclosure) are shown in Table 1.
[0113] Example 3 A polyethylene microporous membrane was produced in the same manner as in Example 1, except that steps (1), (2), and (4) were changed as follows.
[0114] -Step (1)- ・UHMWPE with a Mw of 4.2 million and a Ca content of 31 ppm: 15 parts by mass (UHMWPE powder particle size: 30 μm) ・HDPE with a Mw of 400,000 and a Ca content of 34 ppm: 15 parts by mass (HDPE powder particle size: 20 μm) ・Liquid paraffin: 65 parts by mass ・Decalin: 5 parts by mass The above materials were prepared. Liquid paraffin and decalin were mixed to prepare a mixed solvent. The entire amount of UHMWPE was added to the mixed solvent and stirred and mixed. Next, the entire amount of HDPE was added and stirred and mixed. In this way, a polyethylene solution with a polyethylene concentration of 30% by mass was prepared. The Ca content in the mixture of UHMWPE and HDPE was 32.5 ppm.
[0115] -Step (2)- The polyethylene solution was charged into a twin-screw kneading extruder, and pressure and heat were applied to the polyethylene solution by operating it at a screw rotation speed of 100 rpm. The temperature inside the barrel of the twin-screw kneading extruder was adjusted so that the polyethylene solution temperature in the most downstream region was 175°C, and the polyethylene solution temperature at the die was adjusted so that it was 170°C. The polyethylene solution was extruded from the die in the form of a sheet, and the extrudate was conveyed to a water bath at a water temperature of 20°C and cooled to produce a base tape in the form of a gel-like sheet.
[0116] -Step (4)- The base tape was stretched 5 times in MD at a temperature of 100°C (longitudinal stretching), then stretched 12 times in TD at a temperature of 115°C (transverse stretching), and then immediately heat-set at a temperature of 124°C to obtain a polyolefin microporous membrane.
[0117] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, with numerous micropores inside that were connected to each other, allowing gas or liquid to pass through from one side to the other. The properties of this polyethylene microporous membrane (liquid filter substrate of the present disclosure) are shown in Table 1.
[0118] Example 4 A polyethylene microporous membrane was produced in the same manner as in Example 1, except that steps (1), (2), and (4) were changed as follows.
[0119] -Step (1)- ・UHMWPE with a Mw of 4.2 million and a Ca content of 31 ppm: 18 parts by mass (UHMWPE powder particle size: 30 μm) ・HDPE with a Mw of 400,000 and a Ca content of 34 ppm: 5 parts by mass (HDPE powder particle size: 20 μm) ・Liquid paraffin: 75 parts by mass ・Decalin: 2 parts by mass The above materials were prepared. Liquid paraffin and decalin were mixed to prepare a mixed solvent. The entire amount of UHMWPE was added to the mixed solvent and stirred and mixed. Next, the entire amount of HDPE was added and stirred and mixed. In this way, a polyethylene solution with a polyethylene concentration of 23% by mass was prepared. The Ca content in the mixture of UHMWPE and HDPE was 31.7 ppm.
[0120] -Step (2)- The polyethylene solution was charged into a twin-screw kneading extruder, and pressure and heat were applied to the polyethylene solution by operating it at a screw rotation speed of 220 rpm. The temperature inside the barrel of the twin-screw kneading extruder was adjusted so that the polyethylene solution temperature in the most downstream region was 200°C, and the polyethylene solution temperature at the die was adjusted so that it was 190°C. The polyethylene solution was extruded from the die in the form of a sheet, and the extrudate was conveyed to a water bath at a water temperature of 20°C and cooled to produce a base tape that was a gel-like sheet.
[0121] -Step (4)- The base tape was stretched 9 times in MD at a temperature of 100°C (longitudinal stretching), and then stretched 18 times in TD at a temperature of 105°C (transverse stretching), followed immediately by heat setting at a temperature of 110°C to obtain a polyolefin microporous membrane.
[0122] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, with numerous micropores inside that were connected to each other, allowing gas or liquid to pass through from one side to the other. The properties of this polyethylene microporous membrane (liquid filter substrate of the present disclosure) are shown in Table 1.
[0123] Example 5 A polyethylene microporous membrane was produced in the same manner as in Example 1, except that step (1) and step (6) were changed as follows.
[0124] -Step (1)- UHMWPE with a Mw of 4.6 million and a Ca content of 140 ppb: 4 parts by mass (UHMWPE powder particle size: 60 μm) HDPE with a Mw of 500,000 and a Ca content of 230 ppb: 16 parts by mass (HDPE powder particle size: 250 μm) Liquid paraffin: 80 parts by mass The above materials were prepared. The entire amount of UHMWPE was added to the liquid paraffin and mixed by stirring. Next, the entire amount of HDPE was added and mixed by stirring. In this way, a polyethylene solution with a polyethylene concentration of 20% by mass was prepared. The Ca content in the mixture of UHMWPE and HDPE was 212 ppb.
[0125] -Step (6)- The polyolefin microporous membrane was annealed by conveying it through a thermostatic bath at 115°C for 1 minute while keeping the TD length constant, then conveyed through a space at 60°C for 20 seconds, and then conveyed into a space at room temperature to cool.
[0126] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, with numerous micropores inside that were connected to each other, allowing gas or liquid to pass through from one side to the other. The properties of this polyethylene microporous membrane (liquid filter substrate of the present disclosure) are shown in Table 1.
[0127] Example 6 A polyethylene microporous membrane was produced in the same manner as in Example 1, except that steps (1), (2), and (4) were changed as follows.
[0128] -Step (1)- ・UHMWPE with a Mw of 4.6 million and a Ca content of 140 ppb: 15 parts by mass (UHMWPE powder particle size: 60 μm) ・HDPE with a Mw of 500,000 and a Ca content of 230 ppb: 5 parts by mass (HDPE powder particle size: 250 μm) ・Liquid paraffin: 80 parts by mass The above materials were prepared. The entire amount of UHMWPE was added to the liquid paraffin and mixed by stirring. Next, the entire amount of HDPE was added and mixed by stirring. In this way, a polyethylene solution with a polyethylene concentration of 20% by mass was prepared. The Ca content in the mixture of UHMWPE and HDPE was 162.5 ppb.
[0129] -Step (2)- The polyethylene solution was charged into a twin-screw kneading extruder, and pressure and heat were applied to the polyethylene solution by operating it at a screw rotation speed of 400 rpm. The temperature inside the barrel of the twin-screw kneading extruder was adjusted so that the polyethylene solution temperature in the most downstream region was 200°C, and the polyethylene solution temperature at the die was adjusted so that it was 210°C. The polyethylene solution was extruded from the die in the form of a sheet, and the extrudate was conveyed to a water bath at a water temperature of 20°C and cooled to produce a base tape that was a gel-like sheet.
[0130] -Step (4)- The base tape was stretched 6 times in MD at a temperature of 110°C (longitudinal stretching), and then stretched 13 times in TD at a temperature of 115°C (transverse stretching), followed immediately by heat setting at a temperature of 130°C to obtain a polyolefin microporous membrane.
[0131] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, with numerous micropores inside that were connected to each other, allowing gas or liquid to pass through from one side to the other. The properties of this polyethylene microporous membrane (liquid filter substrate of the present disclosure) are shown in Table 1.
[0132] Comparative Example 1 A polyethylene microporous membrane was produced in the same manner as in Example 1, except that step (2) and step (4) were changed as follows.
[0133] -Step (2)- The polyethylene solution was charged into a twin-screw kneading extruder, and pressure and heat were applied to the polyethylene solution by operating it at a screw rotation speed of 200 rpm. The temperature inside the barrel of the twin-screw kneading extruder was adjusted so that the polyethylene solution temperature in the most downstream region was 160°C, and the polyethylene solution temperature at the die was adjusted so that it was 165°C. The polyethylene solution was extruded from the die in the form of a sheet, and the extrudate was conveyed to a water bath at a water temperature of 20°C and cooled to produce a base tape in the form of a gel-like sheet.
[0134] -Step (4)- The base tape was stretched 9 times in MD at a temperature of 100°C (longitudinal stretching), and then 25 times in TD at a temperature of 105°C (transverse stretching), followed immediately by heat setting at a temperature of 105°C to obtain a polyolefin microporous membrane.
[0135] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibrillar polyolefin, with numerous micropores inside that were connected to each other, allowing gas or liquid to pass through from one side to the other. The properties of this polyethylene microporous membrane are shown in Table 1.
[0136] Comparative Example 2 A polyethylene microporous membrane was produced in the same manner as in Example 1, except that step (4) was changed as follows.
[0137] -Step (4)- The base tape was stretched 9 times in MD at a temperature of 100°C (longitudinal stretching), and then 25 times in TD at a temperature of 115°C (transverse stretching), followed immediately by heat setting at a temperature of 100°C to obtain a polyolefin microporous membrane.
[0138] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibrillar polyolefin, with numerous micropores inside that were connected to each other, allowing gas or liquid to pass through from one side to the other. The properties of this polyethylene microporous membrane are shown in Table 1.
[0139] Comparative Example 3 A polyethylene microporous membrane was produced in the same manner as in Example 1, except that step (1) and step (4) were changed as follows.
[0140] -Step (1)- ・UHMWPE with a Mw of 4.6 million and a Ca content of 140 ppb: 27 parts by mass (UHMWPE powder particle size: 60 μm) ・HDPE with a Mw of 500,000 and a Ca content of 230 ppb: 2 parts by mass (HDPE powder particle size: 250 μm) ・Liquid paraffin: 70 parts by mass ・Decalin: 1 part by mass The above materials were prepared. Liquid paraffin and decalin were mixed to prepare a mixed solvent. The entire amount of UHMWPE was added to the mixed solvent and stirred. Next, the entire amount of HDPE was added and stirred and mixed. In this way, a polyethylene solution with a polyethylene concentration of 29% by mass was prepared. The Ca content in the mixture of UHMWPE and HDPE was 146 ppb.
[0141] -Step (4)- The base tape was stretched 9 times in MD at a temperature of 105°C (longitudinal stretching), and subsequently stretched 25 times in TD at a temperature of 105°C (transverse stretching), followed immediately by heat setting at a temperature of 108°C to obtain a polyolefin microporous membrane.
[0142] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibrillar polyolefin, with numerous micropores inside that were connected to each other, allowing gas or liquid to pass through from one side to the other. The properties of this polyethylene microporous membrane are shown in Table 1.
[0143] Comparative Example 4 A polyethylene microporous membrane was produced in the same manner as in Example 1, except that steps (1), (2), (4), and (6) were changed as follows.
[0144] -Step (1)- UHMWPE with a Mw of 4.2 million and a Ca content of 31 ppm: 3 parts by mass (UHMWPE powder particle size: 30 μm) HDPE with a Mw of 400,000 and a Ca content of 34 ppm: 14 parts by mass (HDPE powder particle size: 20 μm) Liquid paraffin: 51 parts by mass Decalin: 32 parts by mass The above materials were prepared. Liquid paraffin and decalin were mixed to prepare a mixed solvent. The entire amount of UHMWPE was added to the mixed solvent and stirred and mixed. Next, the entire amount of HDPE was added and stirred and mixed. In this way, a polyethylene solution with a polyethylene concentration of 17% by mass was prepared. The Ca content in the mixture of UHMWPE and HDPE was 33.5 ppm.
[0145] -Step (2)- The polyethylene solution was charged into a twin-screw kneading extruder, and pressure and heat were applied to the polyethylene solution by operating it at a screw rotation speed of 450 rpm. The temperature inside the barrel of the twin-screw kneading extruder was adjusted so that the temperature of the polyethylene solution in the most downstream region was 160°C, and the temperature of the polyethylene solution at the die was also adjusted so that it was 160°C. The polyethylene solution was extruded from the die in the form of a sheet, and the extrudate was conveyed to a water bath at a water temperature of 20°C and cooled to produce a base tape that was a gel-like sheet.
[0146] -Step (4)- The base tape was stretched 4 times in MD at a temperature of 100°C (longitudinal stretching), then stretched 9 times in TD at a temperature of 110°C (transverse stretching), and then immediately heat-set at a temperature of 135°C to obtain a polyolefin microporous membrane.
[0147] -Step (6)- The polyolefin microporous membrane was annealed by conveying it through a thermostatic bath at 100°C for 1 minute while keeping the TD length constant, then conveyed it through a space at 60°C for 20 seconds, and then conveyed it into a space at room temperature and cooled.
[0148] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibrillar polyolefin, with numerous micropores inside that were connected to each other, allowing gas or liquid to pass through from one side to the other. The properties of this polyethylene microporous membrane are shown in Table 1.
[0149]
[0150] Comparative Example 4, in which the pore size of the polyolefin microporous membrane was 57 nm, was inferior in the evaluation item "collection performance." In contrast, Examples 1 to 6 (liquid filter substrates of the present disclosure), in which the pore size of the polyolefin microporous membrane was 35 nm or less, were excellent in the evaluation item "collection performance." In other words, the liquid filter substrate of the present disclosure is excellent in the performance of filtering out fine particles (e.g., particles with a particle size of 5 nm) contained in the liquid to be treated.
[0151] Comparative Examples 1 to 3, in which the polyolefin crystallinity was less than 45%, were inferior in the evaluation item "metal elution." In contrast, Examples 1 to 6 (liquid filter substrates of the present disclosure), in which the polyolefin crystallinity was 45% or more, were excellent in the evaluation item "metal elution." In other words, the liquid filter substrate of the present disclosure is easy to remove residual metals by washing, despite its relatively small pore size.
[0152] All publications, patent applications, and technical standards mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, or technical standard was specifically and individually indicated to be incorporated by reference.
[0153] The disclosure of Japanese Application No. 2023-052236, filed on March 28, 2023, is incorporated herein by reference in its entirety.
Claims
1. A substrate for a liquid filter, comprising a microporous polyolefin membrane having a pore size of 1 nm to 35 nm and a crystallinity of the polyolefin of 45% or more.
2. The liquid filter substrate according to claim 1, wherein the polyolefin microporous membrane has a thickness of 3 μm to 20 μm.
3. The liquid filter substrate according to claim 1, wherein the polyolefin microporous membrane has a porosity of 35% to 70%.
4. The water flow rate of the polyolefin microporous membrane is 0.003 L / min / ft 2 / psi to 0.180L / min / ft 2 The liquid filter substrate according to claim 1 , wherein the pressure is 0.1 to 1.0 psi.
5. The liquid filter substrate according to claim 1, wherein the weight average molecular weight of the entire polyolefin constituting said polyolefin microporous membrane is 800,000 or more.
6. The liquid filter substrate according to claim 1, wherein the polyolefin microporous membrane is a polyethylene microporous membrane.
7. A liquid filter comprising the liquid filter substrate according to any one of claims 1 to 6.
Citation Information
Patent Citations
Polyolefin microporous film and its manufacturing method
JP2002128943A
Microporous film
JP2013032490A
Base material for liquid filter
JP2018167198A
Nanoporous ultra-high molecular weight polyethylene membrane