Organopolysiloxane, dispersion, and cosmetic product
The use of an organopolysiloxane with a specific chain length and structure addresses the stickiness and aggregation issues in cosmetics by enhancing powder dispersibility and stability, resulting in improved cosmetic feel and spreadability.
Patent Information
- Application Number
- PCT/JP2024/009458
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-12
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional silicone-based emulsifiers used in cosmetics, such as polyglycerin-modified silicones, tend to be sensually sticky, while fine metal oxide powders in sunscreens aggregate easily due to strong interparticle bonding, leading to stability issues in dispersions.
Development of an organopolysiloxane with a specific chain length and structure that enhances powder dispersibility and stability, allowing for the creation of cosmetics with improved feel and spreadability by modifying the ends of polyglycerin with an organopolysiloxane chain.
The organopolysiloxane provides excellent powder dispersibility and stability, resulting in cosmetics that feel good on the skin and have enhanced spreadability, effectively addressing the aggregation issues of fine metal oxide powders.
Smart Images

Figure JP2024009458_03102024_PF_FP_ABST
Abstract
Description
Organopolysiloxane, dispersion and cosmetic
[0001] The present invention relates to an organopolysiloxane, a dispersion containing the same, and a cosmetic containing the same. In the present invention, compositions for cosmetic preparations may be referred to as "cosmetics."
[0002] Conventionally, silicone-based surfactants have been widely used as emulsifiers for emulsifying silicones. Among them, polyglycerin-modified silicones have the adhesiveness to the skin of polyglycerin and the light feel characteristic of silicone, and are widely used in emulsified cosmetics, etc. However, they are known to tend to cause sensory stickiness (Patent Document 1).
[0003] On the other hand, in sunscreen cosmetics, metal oxide powders such as titanium oxide and zinc oxide are generally used in the form of so-called fine particle metal oxide powders with an average particle size of 100 nm or less in order to improve transparency and enhance UV-shielding effect. However, the surface area of fine particle metal oxide powders is increased, which strengthens the bonding force between particles, and as a result, they tend to aggregate. Therefore, when using such fine particle metal oxide powders in sunscreen cosmetics, it is important that they can be stably contained without aggregation.
[0004] Patent Document 2 proposes a silicone-branched polyglycerin-modified silicone that has high powder dispersibility. However, this structure results in high viscosity. Patent Documents 3 and 4 propose an ABA copolymer as a powder dispersion stabilizer. However, there has been insufficient research into dispersibility due to silicone chain length and its imbalance.
[0005] JP 2002-3334 A, International Publication No. 2016 / 178380, JP 2006-218472 A, JP 2012-207078 A
[0006] The present invention has been made in view of the above circumstances, and aims to provide an organopolysiloxane that exhibits excellent powder dispersibility. Another object of the present invention is to provide a dispersion that exhibits good stability, and a cosmetic that exhibits excellent feel in use and spreadability.
[0007]
[0005] As a result of extensive research aimed at achieving the above object, the present inventors have found that an organopolysiloxane in which each end of a polyglycerol is modified with an organopolysiloxane chain of a specific chain length has excellent powder dispersibility. Furthermore, because the organopolysiloxane has high powder dispersion stability, the present inventors have also found a dispersion containing the organopolysiloxane, which has excellent stability, and a cosmetic composition containing the organopolysiloxane or the dispersion, which has excellent feel in use and spreadability, and have thus completed the present invention.
[0008] Therefore, the present invention provides the following inventions: 1. An organopolysiloxane represented by the following formula (1): [In the formula, R 1 are independently groups selected from an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, and an aralkyl group having 7 to 20 carbon atoms. 2are independently a divalent organic group having 3 to 15 carbon atoms optionally joined via an oxygen atom. p is 0≦p≦9, q is 0≦q≦200, r is 0≦r≦200, m is an integer satisfying 0≦m≦10, n1 is an integer satisfying 0≦n1≦5 (provided that when m=0 or 1, 1≦n1≦5), and n2 is an integer satisfying 0≦n2≦5. However, the bonding of each glycerin unit bracketed by m and n1 may be block or random.] 2. The organopolysiloxane according to 1, wherein in formula (1), n1=0 and m is 0<m≦10. 3. The organopolysiloxane according to 2, wherein in formula (1), p≠q. 4. The organopolysiloxane according to any one of 1 to 3, wherein the organopolysiloxane has a weight average molecular weight, in terms of polystyrene, of 1,000 to 20,000. 5. The organopolysiloxane according to any one of 1 to 4, wherein in formula (1), q satisfies 0≦q≦9 and r satisfies 0≦r≦9. 6. The organopolysiloxane according to any one of 1 to 4, wherein in formula (1), q satisfies 10≦q≦200. 7. A cosmetic preparation comprising the organopolysiloxane according to any one of 1 to 6. 8. A dispersion comprising the organopolysiloxane according to any one of 1 to 6, a powder, and an oil. 9. The dispersion according to 8, wherein the organopolysiloxane according to formula (1) satisfies 0≦q≦9 and r satisfies 0≦r≦9, and the powder has an average primary particle size of less than 15 nm. 10. The dispersion according to 8, wherein the organopolysiloxane according to formula (1) satisfies 10≦q≦200, and the powder has an average primary particle size of 15 nm or more. 11. A cosmetic preparation comprising the dispersion according to any one of 8 to 10.
[0009] According to the present invention, an organopolysiloxane having excellent powder dispersion stability can be provided. When this organopolysiloxane is processed into a powder, a dispersion having excellent stability can be provided. Furthermore, when this organopolysiloxane or a dispersion using this organopolysiloxane is used in a cosmetic, a cosmetic having a good feel in use and excellent spreadability can be provided.
[0010] The present invention will be described in detail below, but is not limited thereto. In the present invention, the use of the present invention in cosmetics will be described in detail below, but the application is not particularly limited. In the present invention, the ingredient name may be written as the cosmetic name or the International Nomenclature of Cosmetic Ingredient (INCI). When the cosmetic name corresponds to the INCI, the cosmetic name or the English name may be omitted.
[0011] [Organopolysiloxane] The organopolysiloxane of the present invention is an organopolysiloxane represented by the following formula (1), and may be used alone or in combination of two or more. [In the formula, R 1 are independently groups selected from an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, and an aralkyl group having 7 to 20 carbon atoms. 2 are independently a divalent organic group having 3 to 15 carbon atoms which may be bonded via an oxygen atom, p is 0≦p≦9, q is 0≦q≦200, r is 0≦r≦200, m is 0≦m≦10, n1 is 0≦n1≦5 (provided that when m=0 or 1, 1≦n1≦5), and n2 is an integer of 0≦n2≦5. However, the bonding of each glycerin unit bracketed by m and n1 may be in block or random form.]
[0012] R 1 are independently groups selected from an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, and an aralkyl group having 7 to 20 carbon atoms. 1 Preferred examples of the alkyl group include an alkyl group having 1 to 15 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aralkyl group having 7 to 10 carbon atoms, and an alkyl group in which some of the hydrogen atoms of the alkyl group have been substituted with fluorine atoms. More specific examples include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, an octyl group, a decyl group, a dodecyl group, a cyclopentyl group, a cyclohexyl group, a phenyl group, a tolyl group, and a trifluoropropyl group. Particularly preferred are an alkyl group having 1 to 5 carbon atoms, a phenyl group, or a trifluoropropyl group.
[0013] R 2are independently divalent organic groups having 3 to 15 carbon atoms which may be bonded via an oxygen atom. 2 are independently divalent organic groups having 3 to 15 carbon atoms which may have an oxygen atom inserted therein. For example, -(CH2)3-, -(CH2)4-, -CH2CH(CH3)CH2-, -(CH2)8-, -(CH2) 11 -, -(CH2)3-O-(CH2)2-, and -(CH2)2-O-(CH2)3-, etc. Among these, -(CH2)3- and -CH2CH(CH3)CH2- are preferred.
[0014] In the above formula, p is 0≦p≦9, preferably 1≦p≦9, and more preferably 3≦p≦9. If p is greater than the upper limit, when used as a dispersant, adsorption to powders is poor and dispersibility deteriorates. q is 0≦q≦200. When blending with the powder described below, if the average primary particle size of the powder is less than 15 nm, 0≦q≦9 is preferred. If q is 9 or less, adsorption to powders and dispersibility are good. Furthermore, if the average primary particle size of the powder is 15 nm or more, 10≦q≦200 is preferred. If q is 10 or more, the hydrophobic group has a necessary and sufficient length, and particles are less likely to aggregate, resulting in good dispersibility. r is 0≦r≦200, and if the average primary particle size of the powder is less than 15 nm, 0≦r≦9 is preferred. If r is 9 or less, adsorption to powders and dispersibility are good. The average primary particle size of the powder was measured by averaging 100 particles randomly selected using a transmission electron microscope (the same applies hereinafter).
[0015] In the above formula, m is 0≦m≦10, preferably 1≦m≦8, and more preferably 1≦m≦5. If m is greater than 10, the polarity will be high when used as a dispersant, which may lead to a deterioration in compatibility between the oil agent and the dispersant, particularly when silicone oil is used as the oil agent. In addition, the viscosity of the dispersant itself will increase, which may result in poor compatibility with the powder and therefore poor dispersibility. Furthermore, n1 is 0≦n1≦5, preferably 0≦n1≦3, more preferably 0≦n1≦1, and even more preferably 0. When n1=0, m is 0<m≦10. When n1 is not 0, n1=1 is preferred. When m=0 or 1, 1≦n1≦5, preferably 1≦n1≦3, and more preferably n1=1. When n1 is 5 or less, the polarity of the dispersant is reduced, which has the effect of increasing the compatibility between the oil agent and the dispersant. n2 is 0≦n2≦5, preferably 1≦n2≦3, and more preferably 1≦n2≦2. If n2 is greater than 5, the polarity of the dispersant becomes high, which may lead to a deterioration in the compatibility between the oil agent and the dispersant, particularly when silicone oil is used as the oil agent. Furthermore, the bonding of each glycerin unit bounded by m and n1 may be block or random. The bonding order of each siloxane unit is not limited.
[0016] In the above formula, organopolysiloxanes in which q is 0≦q≦9 and r is 0≦r≦9 have short siloxane units, exhibit good adsorption to powders with an average primary particle size of less than 15 nm, and have high dispersion stability, and are therefore suitable for use as dispersants for powders with small average primary particle sizes.
[0017] In the above formula, organopolysiloxanes in which q is 10≦q≦200 have long siloxane units, exhibit good adsorption to powders with an average primary particle size of 15 nm or more, and have high dispersion stability, and are therefore suitable for use as dispersants for powders with large average primary particle sizes. As can be seen from these facts, by optimizing the structure, the organopolysiloxane of the present invention can be suitable for use as a dispersant that can well disperse powders of any particle size.
[0018] In the above formula, organopolysiloxanes where n1 = 0 and m is 0 < m ≤ 10 have low viscosity and are capable of uniformly processing powders, making them suitable for use as dispersants. Furthermore, if p ≠ q, then both adsorption to powders and compatibility with oils are satisfactory, resulting in superior powder dispersion stability.
[0019] [Method for Synthesizing Organopolysiloxane] The method for synthesizing the organopolysiloxane of the present invention is not particularly limited, but it can be obtained by subjecting a polyglycerol compound having two or more alkenyl groups as a raw material to an addition reaction with one or more organohydrogenpolysiloxanes having a hydrosilyl group at one end.
[0020] Specifically, they can be obtained by subjecting a polyglycerol compound having two or more alkenyl groups, represented by the following formula (2), to a hydrosilylation reaction with one or more organohydrogenpolysiloxanes having a hydrosilyl group at one end, represented by the following formula (3). The hydrosilylation reaction may also be carried out in the presence of a platinum or rhodium catalyst. [In the formula, R 3 are independently an alkenyl group having 3 to 15 carbon atoms which may have an oxygen atom inserted therein, m is an integer of 0≦m≦10, n1 is an integer of 0≦n1≦5 (provided that when m=0 or 1, 1≦n≦5), and n2 is an integer of 0≦n2≦5, provided that the bonding of each glycerin unit bounded by m and n1 may be in block or random form. [In the formula, R 1 are independently a group selected from an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, and an aralkyl group having 7 to 20 carbon atoms. x is p, q, or r as defined above.
[0021] A polyglycerol compound having two or more alkenyl groups can be obtained by subjecting an epoxy compound such as monoallyl glycidyl ether, monooctenyl glycidyl ether, glycidol, or glycidyl methyl ether to a ring-opening reaction of the epoxy group with a compound having a hydroxyl group such as glycerol, diglycerol, glycerol monoallyl ether, or glycidol in the presence of an alkali catalyst.
[0022] The ring-opening reaction of hydroxyl groups and epoxy groups is known, and the type of alkali catalyst is not particularly limited, but examples that can be used include alkali metal hydroxides such as potassium hydroxide and sodium hydroxide, alkali metal bicarbonates such as sodium bicarbonate and potassium bicarbonate, alkali metal carbonates such as sodium carbonate and potassium carbonate, and sodium methoxide. The amount of alkali catalyst added is 0.2 to 2 mol %, and preferably 0.2 to 1 mol %, based on 100 mol % of the compound having a hydroxyl group. The ring-opening reaction product of the hydroxyl group and the epoxy group contains various isomers depending on the blending composition of the raw materials, and is therefore usually a mixture of these isomers.
[0023] For example, the reaction of 1 mole of glycerin with 2 moles of allyl glycidyl ether theoretically produces the 14 structural isomers shown below.
[0024] The production method by the hydrosilylation reaction is described in more detail below. In the hydrosilylation reaction step between a polyglycerol compound having two or more alkenyl groups represented by the above formula (2) and an organohydrogenpolysiloxane having a hydrosilyl group at one end represented by the above formula (3), the molar ratio of hydrosilyl groups to alkenyl groups is preferably 0.5 to 2.0, and more preferably 0.8 to 1.2.
[0025] This hydrosilylation reaction is preferably carried out in the presence of a platinum catalyst or a rhodium catalyst. Preferred examples include chloroplatinic acid, alcohol-modified chloroplatinic acid, and chloroplatinic acid-vinylsiloxane complexes. Furthermore, since an excessive amount of catalyst will cause coloration of the reaction product, the amount of platinum or rhodium used is preferably 50 ppm (by mass) or less, and more preferably 20 ppm or less.
[0026] Furthermore, the addition reaction may be carried out in the presence of an organic solvent, if necessary. Examples of the organic solvent include cyclic organopolysiloxanes such as octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, and dodecamethylcyclohexasiloxane; aromatic hydrocarbons such as toluene and xylene; ketone-based organic solvents such as acetone, methyl ethyl ketone, diethyl ketone, and methyl isobutyl ketone; aliphatic hydrocarbons such as hexane, heptane, octane, and cyclohexane; monohydric aliphatic alcohols such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-methyl-1-propanol, 2-butanol, 2-methyl-2-propanol, 1-pentanol, 2-methylbutanol, 2-pentanol, 1-hexanol, 2-methylpentanol, 1-heptanol, 1-octanol, 1-nonanol, and 1-decanol; and dihydric aliphatic alcohols such as ethylene glycol and 1,2-propylene glycol. Among these, ethanol, 1-propanol, and 2-propanol are preferred from the viewpoint of reactivity.
[0027] The amount of the solvent used is preferably 1 to 80% by mass, more preferably 5 to 50% by mass, of the entire reaction solution (system). Within this range, the reaction system is maintained uniformly, and the reaction proceeds efficiently.
[0028] The addition reaction conditions are not particularly limited, but it is preferable to heat under reflux at a temperature of 50 to 150°C, more preferably 80 to 120°C, for about 1 to 10 hours.
[0029] After the addition reaction, a step of removing the rhodium catalyst or platinum catalyst used with activated carbon may be included. The amount of activated carbon used is preferably 0.001 to 5.0% by mass, particularly 0.01 to 1.0% by mass, of the entire system. If the amount is within this range, coloration of the reaction product can be further suppressed.
[0030] After the addition reaction, unreacted hydrosilyl groups may remain in the organopolysiloxane. Furthermore, when the organic solvent used in the addition reaction is an aliphatic alcohol, side reactions such as alcohol exchange reactions and dehydrogenation reactions may occur, and alkoxy groups may remain.
[0031] After the addition reaction, if necessary, a step of substituting remaining hydrosilyl groups with hydroxysilyl groups may be included. In particular, when used in applications such as cosmetics, the hydrosilyl groups may be deactivated over time by a dehydrogenation reaction, resulting in the generation of hydrogen gas, which is problematic from the viewpoint of safety. Therefore, it is preferable to include a step of substituting hydrosilyl groups with hydroxysilyl groups.
[0032] A process for substituting hydrosilyl groups with hydroxysilyl groups can involve hydrolyzing unreacted hydrosilyl groups in the presence of a basic catalyst such as an alkali metal carbonate, alkali metal bicarbonate, or alkali metal hydroxide, followed by neutralization by adding an acidic catalyst in an amount equal to the molar equivalent of the basic catalyst. Specific examples of basic catalysts include strong basic catalysts such as lithium hydroxide, sodium hydroxide, potassium hydroxide, calcium hydroxide, and barium hydroxide, and weak basic catalysts such as sodium carbonate, calcium carbonate, and sodium bicarbonate. In terms of promoting the dehydrogenation reaction, it is particularly preferable to use a strong basic catalyst, and sodium hydroxide is particularly preferred. Specific examples of acidic catalysts include inorganic acids such as hydrochloric acid, sulfuric acid, sulfurous acid, fuming sulfuric acid, and phosphoric acid; sulfonic acids such as p-toluenesulfonic acid, methanesulfonic acid, and trifluoromethanesulfonic acid; and carboxylic acids such as formic acid, acetic acid, propionic acid, trifluoroacetic acid, benzoic acid, citric acid, and oxalic acid. In general, it is preferable to use an acid or a base in combination with water and heat at a temperature below the boiling point of water rather than using the acid or base alone. Through this process, hydrosilyl groups (SiH groups) are substituted with hydroxysilyl groups (SiOH groups).
[0033] After the addition reaction, a deodorizing treatment step can be included to reduce odor, if necessary. In particular, when used in applications such as cosmetics, a deodorizing treatment step is preferable due to the tendency for odor to develop over time. The odor-developing mechanism of a typical polyether-modified silicone can be explained as follows: When an addition reaction between an allyl-etherified polyether and a hydrogen polyorganosiloxane is carried out in the presence of a platinum catalyst, a side reaction occurs in which the allyl group undergoes internal rearrangement to produce a propenyl-etherified polyether. This propenyl-etherified polyether has no addition reactivity with the hydrogen polyorganosiloxane and therefore remains in the system as an impurity. When water acts on this propenyl-etherified polyether, the propenyl ether is hydrolyzed, generating propionaldehyde, which is responsible for the unpleasant odor. Furthermore, the above hydrolysis reaction is known to be accelerated in the presence of an acid catalyst. When polyether-modified silicone is used in water-based cosmetics, the liquid becomes more acidic over time due to oxidative degradation of the polyether, accelerating the hydrolysis reaction described above and causing odor.
[0034] There are two typical examples of deodorizing treatment processes: In the first method, an acidic catalyst is added to the solution after the addition reaction to hydrolyze all of the propenyl ether remaining in the system, and the resulting propionaldehyde is distilled off.
[0035] Specific examples of the acid catalyst used in the first formulation include inorganic acids such as hydrochloric acid, sulfuric acid, sulfurous acid, oleum, and phosphoric acid; sulfonic acids such as p-toluenesulfonic acid, methanesulfonic acid, and trifluoromethanesulfonic acid; and carboxylic acids such as formic acid, acetic acid, propionic acid, trifluoroacetic acid, benzoic acid, oxalic acid, and citric acid. These acids are used in combination with water, and when it is necessary to remove the used acid, it is preferable to use an acid with a low boiling point such as hydrochloric acid, formic acid, acetic acid, or trifluoroacetic acid. Furthermore, from the perspective of treatment efficiency, it is preferable to use strong acids such as hydrochloric acid and trifluoroacetic acid, but when a cyclic organopolysiloxane is used as a solvent, there is a risk of ring-opening in the presence of a strong acid, so it is preferable to use a weak acid such as citric acid or acetic acid.
[0036] The treatment temperature is preferably 80° C. or less to prevent oxidation of the hydrophilic groups. The amount of the acidic aqueous solution added is preferably 0.1 to 100% by mass, more preferably 5 to 30% by mass, based on the amount of the organic group-modified organosilicon resin.
[0037] From the viewpoint of productivity, a preferred method is to add an aqueous solution to the reaction solution so that the pH is 7 or less, heat and stir the solution, and then perform strip purification. The strip purification may be carried out at room temperature or under reduced pressure, but the temperature condition is preferably 120° C. or less, and for efficient strip purification under this temperature condition, it is preferable to carry out the strip purification under reduced pressure, or, in the case of normal pressure, under a stream of an inert gas such as nitrogen or argon.
[0038] The second method is to alkylate the unsaturated double bonds by adding hydrogen to the solution after the addition reaction (a so-called hydrogenation reaction), thereby stably controlling the generation of aldehyde compounds over time.
[0039] Hydrogenation reactions can be carried out using hydrogen or metal hydrides, and can also be carried out using homogeneous or heterogeneous reactions. These can be carried out alone or in combination. However, heterogeneous catalytic hydrogenation reactions using solid catalysts are preferred, as they have the advantage that the catalyst used does not remain in the product.
[0040] Examples of solid catalysts include elements or compounds of nickel, palladium, platinum, rhodium, cobalt, chromium, copper, iron, etc. In this case, a catalyst carrier is not necessary, but if one is used, activated carbon, silica, silica alumina, alumina, zeolite, etc. are used. These catalysts can be used alone or in combination. The most preferred catalyst is Raney nickel, which is economically advantageous. Since Raney nickel is usually developed with alkali, it is particularly important to carefully measure the pH of the reaction solution. Furthermore, since the reaction system becomes weakly alkaline, hydrolysis reactions using acidic aqueous solutions are particularly effective for deodorization.
[0041] The hydrogenation reaction is generally preferably carried out at a pressure of 1 to 100 MPa and a temperature of 50 to 200°C. The hydrogenation reaction may be either batchwise or continuous. In the case of a batchwise reaction, the reaction time depends on the amount of catalyst, temperature, etc., but is generally 3 to 12 hours. The hydrogen pressure can be adjusted to a constant pressure as appropriate, but the end point of the hydrogenation reaction is the point at which the hydrogen pressure no longer changes, and can be determined by carefully observing the pressure change.
[0042] The amount of aldehyde contained in the crosslinked organosilicon resin purified by such acid treatment or hydrogenation reaction treatment can be reduced to preferably 70 ppm or less, more preferably 20 ppm or less, and even more preferably 10 ppm or less.
[0043] Furthermore, it is possible to combine the two types of deodorizing treatment steps mentioned above. The acid treatment method can decompose and remove aldehyde compounds, but there is a limit to how completely unsaturated double bonds can be removed, making it impossible to completely suppress the generation of aldehydes, which cause odors. The hydrogenation reaction method can eliminate unsaturated double bonds and thereby reduce the amount of aldehyde compounds generated. However, aldehyde condensates, which are produced by condensation of some of the aldehydes, remain in the system even after the above treatment and are difficult to remove by strip purification. Therefore, complete deodorization is possible by subjecting the solution after the addition reaction to a hydrogenation reaction to alkylate the remaining unsaturated double bonds, and then adding an acid catalyst to decompose the aldehyde condensates in the system.
[0044] [Physical Properties of Organopolysiloxane] The weight average molecular weight of the organopolysiloxane of the present invention is preferably from 1,000 to 20,000, more preferably from 1,000 to 10,000, and even more preferably from 1,000 to 7,000.
[0045] If the weight-average molecular weight of the organopolysiloxane is 1,000 or more, when used as a dispersant, the effect of suppressing the aggregation of powder particles is enhanced. Furthermore, if the weight-average molecular weight is 20,000 or less, the adsorption to powder particles is more sufficient. Furthermore, this range is preferable in terms of performance and workability such as filtration. For these reasons, the molecular weight of the organopolysiloxane of the present invention is preferably 1,000 to 20,000.
[0046] The weight-average molecular weight in the present invention is determined as a weight-average molecular weight converted to polystyrene in gel permeation chromatography (GPC) analysis under the following conditions: [Measurement conditions] Developing solvent: tetrahydrofuran (THF) Flow rate: 0.6 mL / min Detector: differential refractive index detector (RI) Column: TSK Guard column Super H-H TSKgel Super HM-N (6.0 mml.D. x 15 cm x 1) TSKgel Super H2500 (6.0 mml.D. x 15 cm x 1) (all manufactured by Tosoh Corporation) Column temperature: 40°C Sample injection volume: 50 μL (THF solution with a concentration of 0.3% by mass)
[0047] [Dispersion] The organopolysiloxane of the present invention has excellent powder dispersion stability, making it possible to provide a dispersion with excellent stability, for example, powder dispersion, viscosity, and hardness stability. Examples of dispersions include dispersions containing the organopolysiloxane of the present invention, oil, and powder. When the organopolysiloxane of the present invention is used in a dispersion, its amount is determined appropriately, and is preferably 0.1 to 30 mass% of the dispersion containing the organopolysiloxane of the present invention, oil, and powder, more preferably 0.5 to 15 mass%, and even more preferably 1 to 10 mass%. The viscosity of the liquid dispersion at 25°C is not particularly limited, but when produced using a media-agitating mill such as a bead mill, a viscosity of less than 1,000 mPa·s is preferred from the standpoint of ease of bead filtration and ease of incorporation into cosmetics. Furthermore, a viscosity of less than 750 mPa·s is more preferred, and less than 500 mPa·s is even more preferred from the standpoint of usability. The lower limit is not particularly limited, but by setting the viscosity to 100 mPa·s or more, separation of the dispersion into light and dark regions is easily suppressed. The viscosity is measured using a Brookfield viscometer, for example, a spindle LV-2, and indicates the viscosity after 60 seconds at 30 revolutions. The hardness of the paste-like dispersion is also not particularly limited, but when produced using a three-roll mill, a hardness of 100 or less is preferred from the standpoint of ease of processing. Furthermore, from the standpoint of ease of incorporation into cosmetics, a hardness of less than 80 is more preferred, and less than 50 is even more preferred. The lower limit is not particularly limited, but by setting the hardness to 5 or more, separation of the dispersion into light and dark regions is easily suppressed. The hardness indicates a value measured using a rheometer, for example, a Rheometer RT-2002D·D (manufactured by Rheotec Corporation, measurement probe: 10 mmφ, penetration depth: 10 mm, sample stage rising speed: 5 cm / min, temperature: 25°C, range: 200).
[0048] Powder When the organopolysiloxane of the present invention is used in a dispersion, the powder to be dispersed is not particularly limited as long as it is a raw material that can normally be incorporated into cosmetics, but examples include fine particle metal oxide powders, hydrophobically treated color pigments, inorganic powders, metal powders, organic powders, inorganic-organic composite powders, etc. Specific examples are as follows:
[0049] Fine particle metal oxide powder The fine particle metal oxide used in the present invention is one or more selected from fine particles of titanium oxide (display name (INCI: Titanium Dioxide)), iron-containing titanium oxide, zinc oxide (display name (INCI: Zinc Oxide)), cerium oxide (display name (INCI: Cerium Oxide)), and composites thereof. These metal oxides may be composite powders with other powders. The average primary particle size is preferably 200 nm or less, more preferably 120 nm or less. If the particle size is larger than this, the UV protection function will be reduced and white residue will remain.
[0050] The above-mentioned fine particle metal oxide may be untreated or may be surface-treated with a known method commonly used in cosmetics, without any particular limitation. For example, inorganic treatments include silica (display name (INCI: Silica)) coating, alumina (display name (INCI: Alumina)) coating, and aluminum hydroxide (display name (INCI: Aluminum Hydroxide)) coating. Organic treatments include silanes or silylating agents such as triethoxycaprylylsilane (display name (INCI: Triethoxycaprylylsilane)), dimethicone (display name (INCI: Dimethicone)), hydrogen dimethicone (display name (INCI: Hydrogen Dimethicone)), triethoxysilylethyl polydimethylsiloxyethylhexyl dimethicone (display name (INCI: Triethoxysilylethyl Examples of the additive include silicone oils such as Polydimethylsiloxyethyl Hexyl Dimethicone, waxes, paraffins, organic fluorine compounds such as perfluoroalkyl phosphates, surfactants, amino acids such as N-acylglutamic acid, and metal soaps such as aluminum stearate (display name (INCI: Aluminum Stearate)) and magnesium myristate (display name (INCI: Magnesium Myristate)). In particular, triethoxysilylethyl polydimethylsiloxyethyl hexyl dimethicone (display name (INCI: Triethoxysilylethyl Polydimethylsiloxyethyl Hexyl Dimethicone)) is used in sunscreens and foundations because it exhibits high dispersibility in both silicones and oils, while triethoxycaprylylsilane (display name (INCI: Triethoxycaprylylsilane)) and metal soap treatments are preferred in terms of compatibility with component (B) and component (D) described below. These surface treatments may be used alone or in combination of two or more depending on the purpose.
[0051] These surface-treated fine particle metal oxides are also available as commercially available products. For example, fine particle titanium dioxide is commercially available under the trade names STR-100C-LP, STR-100A-LP, STR-100W, STR-100W-LP, STR-100C-LF, STR-40-LP (manufactured by Sakai Chemical Industry Co., Ltd.), MT-N1, MT-01, MT-05, MT-100Z, MT-100TV, MT-100AQ, MT-100WP, MTY-100SAS, MT-150EX, MT-500B, MT-505SAS, MT-700B, MT-700Z, MT-014Z, SMT-500SAS (manufactured by Teika Co., Ltd.), ST-455, ST-455WS, ST-457ECS, ST-495M (manufactured by Titanium Industries Co., Ltd.), and the like. Fine particle zinc oxide products include FINEX-50S-LP2, FINEX-30S-LP2, FINEX-50W, FINEX-30W, FINEX-50W-LP2, FINEX-52W-LP2, FINEX-30W-LP2, FINEX-33W-LP2, FINEX-50-LPT, FINEX-25-LPT, FINEX-50S-LPT, and FINEX-30S-LPT (manufactured by Sakai Chemical Industry Co., Ltd.). These are commercially available under the trade names of MZ-150, MZ-200, MZ-300, MZ-306X, MZX-303S, MZX-303M, MZX-304OTS, MZ-500HP, MZ-505T, MZX-505HPS, MZY-505M, MZ-506X, MZY-203S, MZX-203OTS, MZY-210M3S, TMZ-HA1, and MZX-5080TS (manufactured by Teika).
[0052] When a fine particle metal oxide is blended into a cosmetic containing the organopolysiloxane of the present invention, the blending amount of the fine particle metal oxide is not particularly limited, but is preferably 0.1 to 70% by mass, more preferably 5 to 65% by mass, and even more preferably 45 to 65% by mass, based on the total amount of the dispersion. If the blending amount is less than 0.1% by mass, a sufficient ultraviolet screening effect cannot be obtained, and if the blending amount exceeds 70% by mass, the spreadability during use may be poor, and the cosmetic film may become white or powdery.
[0053] Hydrophobically Treated Color Pigments The hydrophobically treated color pigments are not particularly limited as long as they are pigments that are normally used for coloring cosmetics, and examples thereof include red iron oxide (display name (INCI: Iron Oxides)), yellow iron oxide (display name (INCI: Iron Oxides)), white titanium oxide (display name (INCI: Titanium Dioxide)), black iron oxide (display name (INCI: Iron Oxides)), ultramarines (display name (INCI: Ultramarines)), ferric ferrocyanide (display name (INCI: Ferric Ferrocyanide, Ferric Ammonium Ferrocyanide)), manganese violet (display name (INCI: Manganese Cobalt titanate (Indication name (INCI: Cobalt Titanium Oxide)), chromium hydroxide (Indication name (INCI: Chromium Hydroxide Green)), chromium oxide (Indication name (INCI: Chromium Oxide Greens)), aluminum / cobalt oxide (Indication name (INCI: Cobalt Aluminum Oxide)), titanium / titanium oxide sintered product (Indication name (INCI: Titanium / Titanium Dioxide)), lithium / cobalt titanate (Indication name (INCI: Lithium Cobalt Titanate)), iron oxide / titanium oxide sintered product (Indication name (IRON Any of the following pigments can be used: composites doped with different metals, such as titanium dioxide (display name (INCI: Iron Oxide, Titanium Dioxide)), iron oxide-doped titanium dioxide (display name (INCI: Iron Oxide, Titanium Dioxide)), inorganic brown pigments, such as titanium nitride (display name (INCI: Titanium Nitride)), ferrous hydroxide (display name (INCI: Iron Hydroxide)), γ-iron oxide, inorganic yellow pigments, such as ochre, and colored pigments, such as lakes of tar-based pigments and lakes of natural pigments.
[0054] The shape of the hydrophobized color pigment may be any shape, such as spherical, approximately spherical, rod-like, spindle-like, petal-like, rectangular, or irregular, and there are no particular limitations on its geometric form, as long as it is capable of imparting color to the cosmetic. From the viewpoint of hiding power, a pigment having a particle size, i.e., a volume-average particle size, in the range of 150 to 600 nm is preferable. The volume-average particle size can be measured using a TEM or the like. If the particle size is less than 150 nm, the hiding power is low, which may result in a decrease in the coloring efficiency of the cosmetic, and if the particle size is greater than 600 nm, the feeling during use may be poor.
[0055] Furthermore, the pigment according to the present invention may be partially or completely surface-treated with an inorganic compound such as alumina (display name (INCI: Alumina)), aluminum hydroxide (display name (INCI: Aluminum Hydroxide)), silica (display name (INCI: Silica)), or hydrated silica (display name (INCI: Hydrated Silica)).
[0056] The hydrophobization of a hydrophobically treated color pigment refers to surface treatment of the color pigment with a hydrophobizing agent. The surface hydrophobizing agent for the color pigment according to the present invention is not particularly limited as long as it can impart hydrophobicity, and examples thereof include silicone treatment agents, waxes, paraffins, organic fluorine compounds such as perfluoroalkyl phosphates, surfactants, amino acids such as N-acyl glutamic acid, and metal soaps such as aluminum stearate (display name (INCI: Aluminum Stearate)) and magnesium myristate (display name (INCI: Magnesium Myristate)).
[0057] Among these, silicone treatment agents are preferably used, and examples thereof include silanes or silylating agents such as triethoxycaprylylsilane (labeled as "Triethoxycaprylylsilane" by INCI) or trimethoxysilyl dimethicone (labeled as "Trimethoxysilyl Dimethicone" by INCI), dimethicone (labeled as "Dimethicone" by INCI), hydrogen dimethicone (labeled as "Hydrogen Dimethicone" by INCI), triethoxysilylethyl polydimethylsiloxyethyl hexyl dimethicone (labeled as "Triethoxysilylethyl Polydimethylsiloxyethyl Hexyl ... and silicone compounds such as (Acrylates / Tridecyl Acrylate / Triethoxysilylpropyl Methacrylate / Dimethicone Methacrylate Copolymer (Display name (INCI: Acrylates / Tridecyl Acrylate / Triethoxysilylpropyl Methacrylate / Dimethicone Methacrylate Copolymer)) and (Acrylates / Dimethicone) Copolymer (Display name (INCI: Acrylates / Dimethicone Copolymer)). As the silicone treatment agent, the silicone powder treatment agent described in Japanese Patent No. 3912961 is preferably used, and in particular, triethoxysilylethyl polydimethylsiloxyethyl hexyl dimethicone (displayed as INCI: Triethoxysilylethyl Polydimethylsiloxyethyl Hexyl Dimethicone), which is a dimethylpolysiloxane having triethoxysilyl groups, polydimethylsiloxyethyl groups, and hexyl groups in its side chains, is effectively used because it exhibits high affinity even when the dispersion medium for dispersing the highly hydrophobic treated color pigment is a mixed composition of silicone, hydrocarbon, etc. Note that the above surface hydrophobic treatment agents can be used alone or in combination of two or more.
[0058] In the present invention, the production method for surface-treating a color pigment using a hydrophobic treatment agent is not particularly limited and can be carried out by any known method. Surface treatment methods can be broadly divided into dry methods and wet methods. In the dry method, for example, any stirrer, grinder, mixer, disperser, or the like, such as a Henschel mixer, ball mill, jet mill, kneader, planetary mixer, sand mill, attritor, ribbon blender, disperser mixer, or homomixer, can be used to mix / contact the color pigment used in the present invention with the hydrophobic treatment agent. During this treatment, energy such as heat, mechanochemical mechanical force, or superheated steam may be applied. Alternatively, after thoroughly mixing / contacting the color pigment and the hydrophobic treatment agent, energy such as heat, mechanochemical mechanical force, or superheated steam may be applied separately to carry out the treatment. Alternatively, when mixing / contacting the hydrophobic treatment agent with the color pigment, for the purpose of improving the dispersion efficiency of the hydrophobic treatment agent, a method may be used in which the hydrophobic treatment agent is previously dissolved or dispersed in an arbitrary amount of water, solvent, or supercritical fluid, and then this is sprayed onto the color pigment. As a wet method, the color pigment and the hydrophobic treatment agent are dispersed in water, solvent, or supercritical fluid, mixed / contacted, and then the solvent is evaporated, and further, a treatment can be carried out by separately applying energy such as heating, mechanochemical mechanical force, or superheated steam.
[0059] Specific examples of color pigments that have been subjected to hydrophobic surface treatment include the KTP-09 series, particularly KTP-09W, KTP-09R, KTP-09Y, and KTP-09B (manufactured by Shin-Etsu Chemical Co., Ltd.).
[0060] Inorganic Powders Examples of inorganic powders include zirconium oxide (display name (INCI: Zirconium Dioxide)), zinc oxide (display name (INCI: Zinc Oxide)), cerium oxide (display name (INCI: Cerium Oxide)), magnesium oxide (display name (INCI: Magnesium Oxide)), barium sulfate (display name (INCI: Barium Sulfate)), calcium sulfate (display name (INCI: Calcium Sulfate)), magnesium sulfate (display name (INCI: Magnesium Sulfate)), calcium carbonate (display name (INCI: Calcium Carbonate)), magnesium carbonate (display name (INCI: Magnesium Sulfate)), calcium carbonate (display name (INCI: Calcium Carbonate)), magnesium carbonate (display name (INCI: Magnesium Oxide)), magnesium sulfate ... Carbonate), Talc (InCI: Talc), Cleaved Talc (InCI: Talc), Mica (InCI: Mica), Kaolin (InCI: Kaolin), Sericite (InCI: Mica), Synthetic Fluorphlogopite (InCI: Synthetic Fluorphlogopite), Biotite (InCI: Biotite), Potassium Silicate (InCI: Potassium Silicate), Silica (InCI: Silica), Fumed Silica, Aluminum Silicate (InCI: Aluminum Silicate), Magnesium Silicate (InCI: Magnesium Silicate) Silicate (Al / Mg) (Indication name (INCI: Magnesium Aluminum Silicate)), Calcium silicate (Indication name (INCI: Calcium Silicate)), Silicate (Al / Ca / Na) (Indication name (INCI: Aluminum Calcium Sodium Silicate)), Silicate (Li / Mg / Na) (Indication name (INCI: Lithium Magnesium Sodium Silicate)), Silicate (Na / Mg) (Indication name (INCI: Sodium Magnesium Silicate)), Borosilicate (Ca / Al) (Indication name (INCI: Calcium Aluminum Borosilicate)),Examples of the fine particles include fine particles made of borosilicate (Ca / Na) (display name (INCI: Calcium Sodium Borosilicate)), hydroxyapatite (display name (INCI: Hydroxyapatite)), bentonite (display name (INCI: Bentonite)), montmorillonite (display name (INCI: Montmorillonite)), hectorite (display name (INCI: Hectorite)), zeolite (display name (INCI: Zeolite)), alumina (display name (INCI: Alumina)), aluminum hydroxide (display name (INCI: Aluminum Hydroxide)), boron nitride (display name (INCI: Boron Nitride)), glass (display name (INCI: Glass)), and the like. Examples of inorganic colored pearl pigments include pearl agents such as titanium oxide-coated mica, bismuth oxychloride (display name (INCI: Bismuth Oxychloride)), bismuth oxychloride (display name (INCI: Bismuth Oxychloride)) coated with titanium oxide (display name (INCI: Titanium Dioxide)), talc (display name (INCI: Talc)) coated with titanium oxide (display name (INCI: Titanium Dioxide)), fish scale foil, and colored mica coated with titanium oxide (display name (INCI: Titanium Dioxide)), and are not particularly limited.
[0061] Metal Powder Examples of the metal powder include fine metal particles made of aluminum (display name (INCI: Aluminum Powder)), copper (display name (INCI: Copper Powder)), silver (display name (INCI: Silver Powder)), etc.
[0062] Organic Powders Examples of organic powders include powders made of silicone, polyamide, polyacrylic acid / acrylic acid ester, polyester, polyethylene, polypropylene, polystyrene, styrene / acrylic acid copolymer, divinylbenzene / styrene copolymer, polyurethane, vinyl resin, urea resin, melamine resin, benzoguanamine, polymethylbenzoguanamine, tetrafluoroethylene, polymethyl methacrylate (e.g., polymethyl methacrylate), cellulose, silk, nylon, phenolic resin, epoxy resin, polycarbonate, and the like. In particular, examples of silicones include silicone resin particles (specific examples include polymethylsilsesquioxane (labeled as INCI: Polymethylsilsesquioxane)) and silicone resin-coated silicone rubber powder (specific examples include vinyl dimethicone / methicone silsesquioxane crosspolymer (labeled as INCI: Vinyl Dimethicone / Methicone Silsesquioxane Crosspolymer)) and diphenyl dimethicone / vinyl diphenyl dimethicone / silsesquioxane crosspolymer (labeled as INCI: Diphenyl Dimethicone / Vinyl Diphenyl Dimethicone / Silsesquioxane)). Examples of the stearate include polysilicone-1 crosspolymer (label name (INCI: Polysilicone-1 Crosspolymer)), polysilicone-22 (label name (INCI: Polysilicone-22)), and the like. Metal soaps are also included, and specific examples thereof include zinc stearate (label name (INCI: Zinc Stearate)), aluminum stearate (label name (INCI: Aluminum Stearate)), calcium stearate (label name (INCI: Calcium Stearate)), magnesium stearate (label name (INCI: Magnesium Stearate)), zinc myristate (label name (INCI: Zinc Myristate)), magnesium myristate (label name (INCI: Magnesium Stearate)). Myristate)),Examples also include powders made of cetyl phosphate (zinc / Na) (display name (INCI: Sodium Zinc Cetyl Phosphate)), cetyl phosphate potassium (display name (INCI: Potassium Cetyl Phosphate)), and the like. Further, organic dyes and the like can also be mentioned, and specific examples thereof include Red 3, Red 104(1) (display name (INCI: Red 28, Red 28 Lake)), Red 106, Red 201 (display name (INCI: Red 6)), Red 202 (display name (INCI: Red 7)), Red 204, Red 205, Red 220 (display name (INCI: Red 34)), Red 226 (display name (INCI: Red 30)), Red 227 (display name (INCI: Red 33, RED 33 Lake)), Red 228 (display name (INCI: Red 36)), Red 230(1) (display name (INCI: Red 22, Red 22 Yellow 230 (2), Red 401, Red 505, Yellow 4 (Display name (INCI: Yellow 5)), Yellow 5 (Display name (INCI: Yellow 6, Yellow 6 Lake)), Yellow 202 (1) (Display name (INCI: Yellow 8)), Yellow 203 (Display name (INCI: Yellow 10, Yellow 10 Lake)), Yellow 204 (Display name (INCI: Yellow 11)), Yellow 401 (Display name (INCI:)), Blue 1 (Display name (INCI: Blue 1, Blue 1) Lake)), Blue 2, Blue 201, Blue 205 (display name (INCI: Blue 4), Blue 404, Green 3 (Display name (INCI: Green 3, Green 3 Lake)), Green 201 (Display name (INCI: Green 5)), Green 202 (Display name (INCI: Green 6)), Green 204 (Display name (INCI: Green 8)), Green 205, Orange 201 (Display name (INCI: Orange 5)), Orange 203 (Display name (INCI: Pigment Orange 5)), Orange 204, Orange 205 (Display name (INCI: Orange 4, Orange 4 Lake)), Orange 206 (Display name (INCI: Orange 10)), Orange 207 (Display name (INCI: Orange 11)), cochineal (labeled name (INCI: Cochineal)), laccaic acid (labeled name (INCI: Laccaic Acid)),Examples of natural pigments include safflower red (labeled as INCI: Carthamus Tinctorius (Safflower) Flower Extract), purple root extract (labeled as INCI: Lithospermum Officinale Root Extract), gardenia yellow, and gardenia blue (labeled as INCI: Hydrolyzed Gardenia Florida Extract).
[0063] Inorganic-organic composite powders Examples of inorganic-organic composite powders include composite powders in which the surface of an inorganic powder is coated with an organic powder by a known or commonly used method.
[0064] The amount of powder blended in the dispersion containing the organopolysiloxane of the present invention, oil, and powder is preferably 30 to 90 mass %, more preferably 40 to 85 mass %, and even more preferably 50 to 85 mass %.
[0065] Oil: The oil that is the dispersion medium in which the powder is dispersed by the organopolysiloxane of the present invention is not particularly limited, but it is preferred that the kinematic viscosity at 25°C measured by a Cannon-Fenske viscometer according to the method described in JIS Z 8803:2011 is 1 to 100 mm 2 / s is preferred, and 1 to 30 mm 2 From the viewpoint of compatibility with the organopolysiloxane of the present invention, a kinematic viscosity of 1 to 20 mm 2 More preferred are those of the formula (I) / (II). Specific examples include silicone oil, hydrocarbon oil, ester oil, higher fatty acid, natural oil, and fluorine-based oil. The use of these oils is not limited to being a dispersion medium for powders, and they can be incorporated into cosmetics for a variety of purposes.
[0066] Silicone Oils Examples of silicone oils include trisiloxane (labeled as "Trisiloxane" in INCI), volatile dimethicone (labeled as "Dimethicone" in INCI), low-viscosity dimethicone (labeled as "Dimethicone" in INCI), cyclotetrasiloxane (labeled as "Cyclotetrasiloxane" in INCI), cyclopentasiloxane (labeled as "Cyclopentasiloxane" in INCI), cyclohexasiloxane (labeled as "Cyclohexasiloxane" in INCI), methyl trimethicone (labeled as "Methyl Trimethicone" in INCI), and caprylyl methicone (labeled as "Caprylyl Methicone" in INCI). Methicone), Phenyl Trimethicone (Inci: Phenyl Trimethicone), Methylphenyl Polysiloxane (Inci: Diphenyl Dimethicone), Diphenylsiloxy Phenyl Trimethicone (Inci: Diphenylsiloxy Phenyl Trimethicone), Ethyl Methicone (Inci: Ethyl Methicone), Ethyl Trisiloxane (Inci: Ethyl Trisiloxane), Hydrogen Dimethicone (Inci: Hydrogen Examples of silicone oils that can be used include low-viscosity to high-viscosity linear or branched dimethicones such as amodimethicone (labeled as "Amodimethicone" by INCI) and aminopropyl dimethicone (labeled as "Aminopropyl Dimethicone" by INCI). Among these, examples of commercially available silicone oils include KF-96L-1cs, KF-96L-1.5cs, KF-96L-2cs, KF-96A-6cs, KF-4422, KF-4418, KF-56A, and KF-995 manufactured by Shin-Etsu Chemical Co., Ltd.Other examples include silicone rubbers such as highly polymerized gum-type dimethicone (labeled as "DIMETHICONE" by INCI), gum-type amodimethicone (labeled as "Amodimethicone" by INCI), and gum-type dimethylsiloxane-methylphenylsiloxane copolymers, as well as cyclic organopolysiloxane solutions of silicone gums and rubbers, amino acid-modified silicones, fluorine-modified silicones, silicone resins, and silicone resin solutions. Examples of commercially available silicone oils include KF-54 and KF-54HV. By controlling the compatibility of the organopolysiloxane of the present invention with these oils, it is possible to prepare cosmetics that utilize phase separation technology.
[0067] Hydrocarbon Oils Examples of the hydrocarbon oil include linear and branched hydrocarbon oils, and may be either volatile or non-volatile hydrocarbon oils. Specifically, olefin oligomers (INCI), isododecane (display name (INCI: Isododecane)), dodecane (display name (INCI: Dodecane)), isohexadecane (display name (INCI: Isohexadecane)), undecane (display name (INCI: Undecane)), squalane (display name (INCI: Squalane)), squalene (display name (INCI: Squalene)), mineral oil (display name (INCI: Mineral Oil)), liquid isoparaffin, polyisobutylene (display name), hydrogenated polyisobutene (display name (INCI: Hydrogenated Polyisobutene)), (C13-15) alkanes (display name (INCI: C13-15 Alkane) and the like.
[0068] Ester oils are liquid oils formed by condensing fatty acids having 1 to 20 carbon atoms with alcohols having 1 to 20 carbon atoms, and like the natural oils, they include compositions derived from animals and plants, and examples include polyesters such as monoesters, diesters, and triesters. Specific examples of the alkyl glycol monoisostearates include diisobutyl adipate (label name (INCI: Diisobutyl Adipate)), dihexyldecyl adipate (label name (INCI: Diheptylundecyl Adipate)), isostearyl isostearate (label name (INCI: Isostearyl Isostearate)), isocetyl isostearate (label name (INCI: Isocetyl Isostearate)), trimethylolpropane triisostearate (label name (INCI: Trimethylolpropane Triisostearate)), glycol diethylhexanoate (label name (INCI: Glycol Cetyl ethylhexanoate (InCI: Cetyl Ethylhexanoate), Triethylhexanoin (InCI: Triethylhexanoin), Trimethylolpropane triethylhexanoate (InCI: Trimethylolpropane Triethylhexanoate), Pentaerythrityl tetraethylhexanoate (InCI: Pentaerythrityl Tetraethylhexanoate), Cetyl octanoate (InCI: Cetyl Ethylhexanoate), Octyldodecyl stearoyloxystearate (InCI: Octyldodecyl octyldodecyl esters such as oleyl oleate (labeled as INCI: Oleyl Oleate), octyldodecyl oleate (labeled as INCI: Octyldodecyl Oleate), decyl oleate (labeled as INCI: Decyl Oleate),Neopentyl glycol diethylhexanoate (InCI: Neopentyl Glycol Diethylhexanoate), neopentyl glycol dicaprate (InCI: Neopentyl Glycol Dicaprate), triethyl citrate (InCI: Triethyl Citrate), diethylhexyl succinate (InCI: Diethylhexyl Succinate), amyl acetate (InCI: Amyl Acetate), ethyl acetate (InCI: Ethyl Acetate), butyl acetate (InCI: Butyl Acetate), isocetyl stearate (InCI: Isocetyl Stearate), Butyl stearate (InCI: Butyl Stearate), Diisopropyl sebacate (InCI: Diisopropyl Sebacate), Diethylhexyl sebacate (InCI: Diethylhexyl Sebacate), Cetyl lactate (InCI: Cetyl lactate), Myristyl lactate (InCI: Myristyl lactate), Isononyl isononanoate (InCI: Isononyl isononanoate), Isotridecyl isononanoate (InCI: Isotridecyl Coco-Caprylate / Caprate (INCI: Coco-Caprylate / Caprate)), Caprylic / Capric Triglyceride (INCI: Caprylic / Capric Triglyceride), Isopropyl Palmitate (INCI: Isopropyl Palmitate)), Ethylhexyl Palmitate (INCI: Ethylhexyl Isopalmitate)), Hexyldecyl Palmitate (INCI: Isocetyl Palmitate, Hexyldecyl palmitate esters such as cholesteryl hydroxystearate (labeled name (INCI: Cholesteryl Hydroxystearate));Myristate esters such as isopropyl myristate (label name (INCI: Isopropyl Myristate)), octyldodecyl myristate (label name (INCI: Octyldodecyl Myristate)), and myristyl myristate (label name (INCI: Myristyl Myristate)), ethylhexyl laurate (label name (INCI: Ethylhexyl Laurate)), hexyl laurate (label name (INCI: Hexyl Laurate)), and dioctyldodecyl lauroyl glutamate (label name (INCI: Dioctyldodecyl Lauroyl Glutamate)), Examples of glyceride oils include glyceride oils such as lauroyl sarcosine isopropyl ester (label name (INCI: Isopropyl Lauroyl Sarcosinate)), diisostearyl malate (label name (INCI: Diisostearyl Malate)), glyceryl acetate (label name (INCI: Glyceryl Acetate)), and glyceryl stearate (label name (INCI: Glyceryl Stearate)).
[0069] Higher Fatty Acids Examples of higher fatty acids include oleic acid (labeled as "Oleic Acid" in INCI), linoleic acid (labeled as "Linoleic Acid" in INCI), linolenic acid (labeled as "Linolenic Acid" in INCI), arachidonic acid (labeled as "Arachidonic Acid" in INCI), eicosapentaenoic acid (EPA) (labeled as "Eicosapentaenoic Acid" in INCI), docosahexaenoic acid (DHA) (labeled as "Docosahexaenoic Acid" in INCI), isostearic acid (labeled as "Isostearic Acid" in INCI), and hydroxystearic acid (labeled as "Hydroxystearic Acid" in INCI).
[0070] ・Natural oils Natural oils and fats of natural animals and plants and semi-synthetic oils and fats Specific oils and oils (indicated names (INCI: Perseea) Gratissima (Avocado) Oil), アマニoil (indicated name (INCI: Linum) Usitatissimum (Linseed) Seed Oil)), アーモンド oil (indicated name (INCI: Prunus AmスggallsDulces (Sweet Almond) Oil), オリーブoil (indicated name (INCI: Olea Europaea (Olive) Fruit Oil)), アメリカガヤ oil (indicated name (INCI: Torreya Californica (California Nutmeg) Oil)), コウスイガヤ oil (indicates the name (INCI: Cymbopogon (Citronella) Oil)), サメ liver oil (indicated name (INCI: Shark Liver) Oil)), タラ liver oil (indicated name (INCI: Cod Liver Oil), Cod Liver Oil (Indication Name (INCI: Fish Liver Oil)), Kyownin Oil (Indication Name (INCI: Kyounnin Yuu)), Goma Oil (Indication Name (INCI: Sesamumum Indicum (Sesame) Seeded Oil)), Comerm Oil (Indication Name (INCI: Oryza Sativa (Rice) Germ Oil)), Comed Nut Oil (Indication Name (INCI: Oryza Sativa (Rice) Bran Oil), safflower oil (Indication name (INCI: Camellia Kissii Seed Oil)), tatur oil (Indication name (INCI: Turtle Oil)), tsubaki oil (Indication name (INCI: Camellia Japonica Seed Oil)), evening primrose oil (Indication name (INCI: Oenothera Biennis (Evening Primrose) Oil)), tomorokoshi germ oil (Indication name (INCI: Zea Mays (Corn) Germ Oil))、Natan oil(Indication name(INCI:RAPE SHUSHI YU))、Comugi germ oil(Indication name(INCI:Triticum Vulgare (Wheat) Germ Oil))、Parshku oil(Indication name(INCI: ))、Palm oil (indication name (INCI: Elaeis Guineensis (Palm) Oil)), palm kernel oil (indication name (INCI: Elaeis Guineensis (Palm) Kernel Oil)), castor oil (indication name (INCI: Ricinus) Communis (Castor) Seed Oil)), hydrogenated castor oil (label name), sunflower seed oil (label name (INCI: Helianthus Annuus (Sunflower) Seed Oil)), grape seed oil (label name (INCI: Vitis)) Vinifera (Grape Seed Oil)), Jojoba Seed Oil (Display name (INCI:Simmondsia) Chinensis (Jojoba Seed Oil)), Macadamia nut oil (Indication name (INCI: Macadamia Ternifolia Seed Oil)), Mink oil (Indication name (INCI: Mink) Meadowfoam oil (INCI: Limnanthes Alba (Meadowfoam) Seed Oil)), cottonseed oil (INCI: Gossypium Herbaceum (Cotton) Seed) Coconut oil (Indication name: INCI: Cocos Nucifera (Coconut) Examples of the oils that can be used include hydrogenated coconut oil (labeled as INCI: Hydrogenated Coconut Oil), egg yolk oil (labeled as INCI: Egg Oil), and Argania spinosa kernel oil (labeled as INCI: Argania Spinosa Kernel Oil).
[0071] Fluorine-Based Oils Examples of fluorine-based oils include perfluoropolyethers such as polyperfluoromethylisopropyl ether (labeled as Polyperfluoromethylisopropyl Ether by INCI), and perfluorocarbons such as perfluorodecalin (labeled as Perfluorodecalin by INCI) and perfluorohexane (labeled as Perfluorohexane by INCI).
[0072] The blend amount of oil is preferably 9 to 69 mass %, more preferably 14 to 50 mass %, and even more preferably 14 to 45 mass %, of the dispersion containing the organopolysiloxane of the present invention, oil, and powder.
[0073] [Method for Producing Dispersion] A preferred method for preparing a dispersion is to premix powders with the organopolysiloxane of the present invention and oil. Depending on the viscosity of the dispersion to be prepared, a suitable dispersing machine may be selected from a triple roll mill, a homomixer, a disperser, a media agitation mill such as a bead mill, a wet high-pressure disperser, an ultrasonic disperser, or the like.
[0074] [Cosmetics] There are no particular limitations on the cosmetic, as long as it contains the organopolysiloxane of the present invention. When blending powder into a cosmetic containing the organopolysiloxane of the present invention, it can be blended into the cosmetic in the same way as other ingredients without any prior treatment, but if higher dispersibility in the cosmetic is desired, it is preferable to prepare a dispersion in which the powder is previously mixed with other ingredients and then blend this.
[0075] When the organopolysiloxane of the present invention is used in cosmetics, it can be used alone or in combination of two or more. As described above, the organopolysiloxane of the present invention has excellent powder dispersibility, but its use in cosmetics is not limited to dispersants. For example, it can be used as an emulsifier when preparing water-in-oil emulsions, as a stabilizer for oil-in-water emulsions, or as a texture modifier or compatibilizer for non-aqueous formulations. The amount of organopolysiloxane blended is preferably in the range of 0.1 to 40% by mass of the total cosmetic, and as an emulsifier, it is more preferably in the range of 0.1 to 5% by mass of the total cosmetic. Even when blended as a dispersion, the amount of the organopolysiloxane can be appropriately adjusted so that it falls within the above range. By using the organopolysiloxane and dispersion, the cosmetic of the present invention becomes a cosmetic with excellent usability, spreadability, and preferably stability.
[0076] In addition to the oil and powder, the cosmetic of the present invention can contain various components commonly used in cosmetics to the extent that the effects of the present invention are not impaired. For example, the cosmetic may contain (1) an oil, (2) an aqueous component, (3) a surfactant, (4) a powder, (5) a composition consisting of a crosslinked organopolysiloxane and an oil that is liquid at room temperature, (6) a film-forming agent, and (7) other additives. These may be used alone or in appropriate combinations of two or more, each in an appropriate amount. The cosmetic may also contain the powder and oil exemplified above for the dispersion.
[0077] (1) Oil Agent The oil agent may be volatile or non-volatile and may be solid, semi-solid, or liquid at room temperature (25°C). Examples of the oil agent include the oils described above, as well as the oils used in the dispersion, components that are solid or semi-solid at room temperature (25°C), and ultraviolet absorbers.
[0078] The oily component that is solid at 25°C preferably has a melting point of 40°C or higher, more preferably 60 to 110°C, and examples thereof include waxes, hydrocarbons, esters, higher alcohols, and higher fatty acids. These may be any raw materials that can be incorporated into ordinary cosmetics, and are not particularly limited. Specific examples include carnauba wax, sugarcane wax, candelilla wax, refined candelilla wax, rice wax, Japan wax, jojoba wax, kapok wax, rice bran wax, white bayberry fruit wax, shea butter, cacao butter, vegetable waxes such as Rhus Succedanea Fruit Wax (INCI: Rhus Succedanea Fruit Wax), montan wax (INCI: Montan Wax), and hydrogenated castor oil isostearate, beeswax, beef tallow, beef bone fat, lard (INCI: Lard), and horse fat (INCI: Horse Fat). Fat), sheep tallow, lanolin (INCI: Lanolin), animal waxes such as butterbur, shellac wax, and spermaceti; semi-synthetic waxes such as lanolin esters, lanolin fatty acid esters, and beeswax acid esters; hydrogenated oils such as hydrogenated castor oil and hydrogenated coconut oil; solid paraffin, polyethylene, ceresin, ozokerite, and hydrocarbon waxes such as microcrystalline wax; higher alcohols such as stearyl alcohol, behenyl alcohol, and cetanol; wax esters such as synthetic beeswax; amino acid stearyl alcohols such as dioctyldodecyl lauroyl glutamate, dioctyldodecyl lauroyl glutamate, and dioctyldodecyl lauroyl glutamate; fatty acids such as stearic acid and behenic acid; and silicone waxes such as acrylic silicone resins of acrylic-silicone graft or block copolymers (Shin-Etsu Chemical Co., Ltd.: acrylic-silicone graft copolymer: KP-561P, etc.), or derivatives thereof, and it is preferable to use one or more selected from these.
[0079] Examples of ultraviolet absorbers include oxybenzone-1 (label name (INCI: Benzophenone-1)), oxybenzone-2 (label name (INCI: Benzophenone-2)), oxybenzone-3 (label name (INCI: Benzophenone-3)), oxybenzone-4 (label name (INCI: Benzophenone-4)), oxybenzone-5 (label name (INCI: Benzophenone-5)), oxybenzone-6 (label name (INCI: Benzophenone-6)), oxybenzone-9 (label name (INCI: Benzophenone-9)), homosalate (INCI), octocrylene (INCI), t-butyl methoxydibenzoylmethane (label name (INCI: Butyl (Inc. Isopropyl alcohol)), ethylhexyl salicylate (Inc. Isopropyl alcohol), diethylamino hydroxybenzoyl hexyl benzoate (Inc. Isopropyl alcohol), polysilicone-15 (Inc. Isopropyl alcohol), dimethoxybenzylidene dioxoimidazolidine octyl propionate (Inc. Isopropyl alcohol), terephthalylidene dicamphorsulfonic acid (Inc. Isopropyl alcohol), Dicamphor Sulfonic Acid), Ethylhexyl Triazone (INCI), Methyl Bis(trimethylsiloxy)silylisopentyl Trimethoxycinnamate (InCI: Isopentyl Trimethoxycinnamate Trisiloxane), Drometrizole Trisiloxane (INCI), Ethylhexyl Dimethyl PABA (InCI: Ethylhexyl Dimethyl PABA), Isopropyl Paramethoxycinnamate (InCI: Isopropyl Methoxycinnamate), Ethylhexyl Methoxycinnamate (InCI: Ethylhexyl Methoxycinnamate),Bis-ethylhexyloxyphenol methoxyphenyl triazine (INCI), phenylbenzimidazole sulfonic acid (label name (INCI: Phenylbenzimidazole Sulfonic Acid)), methylene bisbenzotriazolyl tetramethylbutylphenol (INCI), glyceryl dimethoxycinnamate ethyl hexanoate (label name (INCI: Glyceryl Ethylhexanoate Dimethoxycinnamate)), glyceryl PABA (INCI), methyl diisopropylcinnamate (label name (INCI: Diisopropyl Methyl Cinnamate)), cinoxate (INCI), ethylhexyl dimethoxybenzylidene dioxoimidazolidinepropionate (label name (INCI: Ethylhexyl Dimethoxybenzylidine Dioxoimidazolidine Propionate). It is also possible to use a UVA absorber (e.g., diethylaminohydroxybenzoyl hexyl benzoate) and a UVB absorber (e.g., ethylhexyl methoxycinnamate) in combination, and these can also be combined in any desired manner.
[0080] The blending amount of the oil in the cosmetic is preferably 1 to 85% by mass, more preferably 3 to 30% by mass, and even more preferably 5 to 20% by mass.
[0081] (2) Aqueous Component The aqueous component is not particularly limited as long as it is an aqueous component that can be typically incorporated into cosmetics. Specific examples include water, lower alcohols preferably having 2 to 5 carbon atoms, such as ethanol (labeled as "Alcohol" in C1C) and isopropanol (labeled as "Isopropyl Alcohol" in C1C), and sugar alcohols, such as sorbitol (C1C), maltose (C1C), and xylitol (C1C). Further, polyhydric alcohols such as BG (display name (INCI: Butylene Glycol)), PG (display name (INCI: Propylene Glycol)), DPG (display name (INCI: Dipropylene Glycol)), pentylene glycol (INCI), 1,10-decanediol (INCI), octanediol (INCI), 1,2-hexanediol (INCI), erythritol (INCI), glycerin (INCI), diglycerin (INCI), and polyethylene glycol; glucose (INCI), glyceryl glucoside (INCI), betaine (INCI), sodium chondroitin sulfate (display name (INCI: Sodium Chondroitin Sulfate)), PCA-Na (display name (INCI: Sodium Examples of moisturizing agents include PCA), methyl gluceth-10 (INCI), methyl gluceth-20 (INCI), hyaluronic acid, egg yolk lecithin, soybean lecithin, phosphatidylcholine, phosphatidylethanolamine, phosphatidylserine, phosphatidylglycerol, phosphatidylinositol, and sphingophospholipid. The remaining amount may be water.
[0082] (3) Surfactants Surfactants include nonionic, anionic, cationic, and amphoteric surfactants, but are not particularly limited, and any surfactants commonly used in cosmetics can be used. Among these surfactants, one or more selected from non-crosslinked silicone surfactants and crosslinked silicone surfactants are preferred in terms of obtaining stable cosmetics. In either case, the amount of surfactant blended is preferably 0.1 to 20% by mass of the total cosmetic. If it is 0.1% or more, the dispersion and emulsification functions can be fully performed, and if it is 20% by mass or less, the cosmetic will not feel sticky after use. The HLB of the surfactant is not limited, but is preferably 2 to 14.5 in order to maintain the water resistance of the cosmetic.
[0083] The non-crosslinked silicone surfactant is one in which some of the methyl groups in a linear or branched silicone main chain have been substituted with hydrophilic groups such as polyethylene glycol or polyglycerin, and specifically, preferred are linear or branched polyoxyethylene-modified organopolysiloxanes, linear or branched polyoxyethylene-polyoxypropylene-modified organopolysiloxanes, linear or branched polyoxyethylene-alkyl-co-modified organopolysiloxanes, linear or branched polyoxyethylene-polyoxypropylene-alkyl-co-modified organopolysiloxanes, linear or branched polyglycerin-modified organopolysiloxanes, linear or branched polyglycerin-alkyl-co-modified organopolysiloxanes, and linear or branched pyrrolidone-modified organopolysiloxanes. Examples of suitable dimethicones include PEG-11 methyl ether dimethicone (INCI), PEG / PPG-20 / 22 butyl ether dimethicone (INCI), PEG-3 dimethicone (INCI), PEG-10 dimethicone (INCI), PEG-9 polydimethylsiloxyethyl dimethicone (INCI), lauryl PEG-9 polydimethylsiloxyethyl dimethicone (INCI), cetyl PEG / PPG-10 / 1 dimethicone (INCI), polyglyceryl-3 disiloxane dimethicone (INCI), polyglyceryl-3 polydimethylsiloxyethyl dimethicone (INCI), lauryl polyglyceryl-3 polydimethylsiloxyethyl dimethicone (INCI), and bis-butyl dimethicone polyglyceryl-3 (INCI).
[0084] Commercially available examples include KF-6011, KF-6011P, KF-6012, KF-6015, KF-6017, KF-6043, KF-6028, KF-6038, KF-6048, KF-6100, KF-6104, KF-6106, KF-6105, and KF-6115 manufactured by Shin-Etsu Chemical Co., Ltd.
[0085] Examples of crosslinked silicone surfactants include crosslinked polyether-modified silicones such as (dimethicone / (PEG-10 / 15)) crosspolymer (INCI), (PEG-15 / lauryl dimethicone) crosspolymer (INCI), (PEG-10 / lauryl dimethicone) crosspolymer (INCI), and (PEG-15 / lauryl polydimethylsiloxyethyl dimethicone) crosspolymer (INCI); and crosslinked polyglycerin-modified silicones such as (dimethicone / polyglycerin-3) crosspolymer (INCI), (lauryl dimethicone / polyglycerin-3) crosspolymer (INCI), and (polyglycerin-3 / lauryl polydimethylsiloxyethyl dimethicone) crosspolymer (INCI).
[0086] Furthermore, when a crosslinked silicone surfactant is used, in a composition comprising the crosslinked silicone surfactant and an oily agent that is liquid at room temperature, it is preferable that the crosslinked silicone surfactant swells with the liquid oil in an amount equal to or greater than its own weight.
[0087] The liquid oil may be any of the liquid silicone oils, hydrocarbon oils, ester oils, natural animal and vegetable oils, semi-synthetic oils, and fluorine-based oils exemplified above as oils, etc., and examples thereof include cyclopentasiloxane (INCI), dimethicone (INCI), mineral oil (INCI), isododecane (INCI), isohexadecane (INCI), triethylhexanoin (INCI), isotridecyl isononanoate (display name (INCI: Isotridecyl Isononanoate)), squalane (INCI), and the like. Examples of commercially available cross-linked silicone surfactants that swell when exposed to a liquid oil include KSG-210, KSG-240, KSG-270, KSG-310, KSG-320, KSG-330, KSG-340, KSG-320Z, KSG-350Z, KSG-710, KSG-810, KSG-820, KSG-830, KSG-840, KSG-820Z, and KSG-850Z manufactured by Shin-Etsu Chemical Co., Ltd.
[0088] (4) Powder Powders can be blended together with the organopolysiloxane as a dispersion, or can be used separately. Alternatively, they can be blended into cosmetics as other dispersions. Specific examples of dispersions in which particles that absorb and scatter ultraviolet light are pre-dispersed in an oil include the SPD series (trade names) manufactured by Shin-Etsu Chemical Co., Ltd., in particular SPD-T5, T5L, Z5, Z5L, T6, Z6, T7, and Z7L.
[0089] The blending amount of the powder in the cosmetic is preferably 0.5 to 90% by mass, more preferably 1 to 30% by mass, and even more preferably 5 to 20% by mass.
[0090] (5) Compositions Comprising Crosslinked Organopolysiloxanes and Oils Liquid at Room Temperature In compositions comprising a crosslinked organopolysiloxane and an oil that is liquid at room temperature, the crosslinked organopolysiloxane preferably swells with the liquid oil in an amount equal to or greater than its own weight. Examples of such liquid oils include the liquid silicone oils, hydrocarbon oils, ester oils, natural animal and vegetable oils, and semi-synthetic oils listed above, as well as fluorine-containing oils. Examples of such liquid oils include cyclopentasiloxane (INCI), dimethicone (INCI), mineral oil (INCI), isododecane (INCI), isohexadecane (INCI), triethylhexanoin (INCI), isotridecyl isononanoate (labeled name: INCI: Isotridecyl Isononanoate), and squalane (INCI).
[0091] Unlike the crosslinked silicone surfactant of component (3) described above, component (5) is a compound that does not have a polyether or polyglycerin structure in its molecular structure, and specific examples include (dimethicone / vinyl dimethicone) crosspolymer (INCI), (dimethicone / phenyl vinyl dimethicone) crosspolymer (INCI), (vinyl dimethicone / lauryl dimethicone) crosspolymer (INCI), (lauryl polydimethylsiloxyethyl dimethicone / bis vinyl dimethicone) crosspolymer (INCI), etc. Examples of commercially available compositions comprising a crosslinked organopolysiloxane and an oil that is liquid at room temperature include KSG-15, KSG-1510, KSG-16, KSG-1610, KSG-19, KSG-016F, KSG-18A, KSG-41A, KSG-42A, KSG-43, KSG-44, KSG-042Z, KSG-045Z, and KSG-048Z, all manufactured by Shin-Etsu Chemical Co., Ltd.
[0092] (6) Film-Forming Agent The film-forming agent is blended mainly for the purpose of further maintaining the durability of the cosmetic effect. Although there are no particular limitations, a silicone-based composition is preferable from the viewpoint of imparting water repellency. Specifically, trimethylsiloxysilicate, crosslinked trimethylsiloxysilicate, modified trimethylsiloxysilicate, acrylic-silicone film-forming agent, silicone-modified norbornene, silicone-modified pullulan, silicone-modified polyvinyl alcohol, etc. can be used. Examples of film-forming agents for silicone-based compositions include trimethylsiloxysilicate (labeled as (INCI): Trimethylsiloxysilicate), (Acrylates / Dimethicone) Copolymer (INCI), (Norbornene / Tris(trimethylsiloxy)silylnorbornene) Copolymer (INCI), tri(trimethylsiloxy)silylpropylcarbamate pullulan (labeled as (INCI): Trimethylsiloxysilylcarbamoyl Pullulan)), and the like.
[0093] The film-forming agent may be dissolved in a liquid oil at room temperature before blending into the cosmetic. Examples of such liquid oil include liquid silicone oils, hydrocarbon oils, ester oils, natural animal and vegetable oils, semi-synthetic oils, and fluorine-based oils, all of which are included in the optional component (1) oil. Specific examples of commercially available silicone film-forming agents include KF-7312J, KP-545, KP-549, KP-543, NBN-30-ID, TSPL-30-ID, and TSPL-30-D5 manufactured by Shin-Etsu Chemical Co., Ltd.
[0094] (7) Other additives Examples of other additives include oil-soluble gelling agents, preservatives / disinfectants, antiperspirants, fragrances, salts, antioxidants, pH adjusters, chelating agents, cooling agents, anti-inflammatory agents, skin-beautifying ingredients (skin-whitening agents, cell activators, skin roughness improving agents, blood circulation promoters, skin astringents, antiseborrheic agents, etc.), vitamins, amino acids, nucleic acids, hormones, and inclusion compounds.
[0095] Oil-soluble gelling agents include metal soaps such as aluminum stearate, magnesium stearate, and zinc myristate; amino acid derivatives such as lauroyl glutamic acid (labeled as "Lauroyl Glutamic Acid" by INCI) and α,γ-di-n-butylamine; dextrin palmitate (labeled as "Dextrin Palmitate" by INCI), dextrin isostearate (labeled as "Dextrin Isostearate" by INCI), dextrin myristate (labeled as "Dextrin Myristate" by INCI), inulin stearate (labeled as "Stearoyl Inulin" by INCI), and dextrin (palmitate / ethylhexanoate) (labeled as "Dextrin" by INCI). dextrin fatty acid esters such as dextrin palmitate / ethylhexanoate); sucrose fatty acid esters such as sucrose palmitate and sucrose stearate; fructooligosaccharide fatty acid esters such as fructooligosaccharide stearate and fructooligosaccharide 2-ethylhexanoate; benzylidene derivatives of sorbitol such as monobenzylidene sorbitol and dibenzylidene sorbitol; disteardimonium hectorite (INCI), stearalkonium hectorite (INCI), organically modified clay minerals of hectorite; and stearalkonium bentonite (INCI).
[0096] - Preservatives and disinfectants Examples of preservatives and disinfectants include alkyl parahydroxybenzoate, benzoic acid, sodium benzoate, sorbic acid, potassium sorbate, phenoxyethanol, imidazolidinyl urea, salicylic acid, isopropylmethylphenol, carbolic acid, parachlormetacresol, hexachlorophene, benzalkonium chloride, chlorhexidine chloride, trichlorocarbanilide, iodopropynyl butylcarbamate, polylysine, photosensitizers, silver, plant extracts, etc.
[0097] Antiperspirants include aluminum hydroxyhalides such as chlorohydroxy AL, aluminum halides such as aluminum chloride, aluminum allantoin, tannic acid, persimmon tannin, sulfuric acid (AL / K), zinc oxide, zinc paraphenolsulfonate, burnt alum, tetrachloro(Al / zirconium) hydrate, trichlorohydrex glycine (Al / zirconium), etc. Particularly preferred components that exhibit high effectiveness are aluminum hydroxyhalides, aluminum halides, and complexes or mixtures thereof with zirconyl oxyhalides and zirconyl hydroxyhalides (for example, tetrachloro(Al / zirconium) hydrate, trichlorohydrex glycine (Al / zirconium)).
[0098] Fragrances Fragrances include natural fragrances and synthetic fragrances. Natural fragrances include plant-based fragrances isolated from flowers, leaves, wood, peels, etc.; and animal-based fragrances such as musk and civet. Synthetic fragrances include hydrocarbons such as monoterpenes, alcohols such as aliphatic alcohols and aromatic alcohols, aldehydes such as terpene aldehydes and aromatic aldehydes, ketones such as alicyclic ketones, esters such as terpene esters, lactones, phenols, oxides, nitrogen-containing compounds, and acetals.
[0099] Salts Examples of salts include inorganic salts, organic acid salts, amine salts, and amino acid salts. Examples of inorganic salts include sodium salts, potassium salts, magnesium salts, calcium salts, aluminum salts, zirconium salts, and zinc salts of inorganic acids such as hydrochloric acid, sulfuric acid, carbonic acid, and nitric acid; examples of organic acid salts include salts of organic acids such as acetic acid, dehydroacetic acid, citric acid, malic acid, succinic acid, ascorbic acid, and stearic acid; examples of amine salts and amino acid salts include salts of amines such as triethanolamine, and salts of amino acids such as glutamic acid. In addition, salts of hyaluronic acid, chondroitin sulfate, aluminum zirconium glycine complexes, and even acid-alkali neutral salts used in cosmetic formulations can also be used.
[0100] Antioxidants Examples of antioxidants include, but are not limited to, carotenoids, ascorbic acid and its salts, ascorbyl stearate, tocopherol, tocopherol acetate, tocopherol, p-t-butylphenol, butylhydroxyanisole, dibutylhydroxytoluene, phytic acid, ferulic acid, thiotaurine, hypotaurine, sulfites, erythorbic acid and its salts, chlorogenic acid, epicatechin, epigallocatechin, epigallocatechin gallate, apigenin, campherol, myricetin, quercetin, etc. One type of antioxidant may be used alone, or two or more types may be used in combination.
[0101] pH Adjusting Agents Examples of pH adjusting agents include lactic acid, citric acid, glycolic acid, succinic acid, tartaric acid, dl-malic acid, potassium carbonate, sodium bicarbonate, and ammonium bicarbonate.
[0102] Chelating Agents Examples of chelating agents include alanine, edetate sodium salt, sodium polyphosphate, sodium metaphosphate, phosphoric acid, and the like.
[0103] Cooling agents include L-menthol, camphor, menthyl lactate, and the like.
[0104] Anti-inflammatory Agents Examples of anti-inflammatory agents include allantoin, glycyrrhizinic acid and its salts, glycyrrhetinic acid and stearyl glycyrrhetinate, tranexamic acid, and azulene.
[0105] Skin-beautifying ingredients Examples of skin-beautifying ingredients include whitening agents such as placenta extract, arbutin, glutathione, and saxifrage extract; cell activators such as royal jelly, photosensitizers, cholesterol derivatives, and calf blood extract; rough skin improving agents; blood circulation promoters such as nonylic acid valenylamide, nicotinic acid benzyl ester, nicotinic acid β-butoxyethyl ester, capsaicin, zingerone, cantharides tincture, ichthammol, caffeine, tannic acid, α-borneol, tocopherol nicotinate, inositol hexanicotinate, cyclandelate, cinnarizine, tolazoline, acetylcholine, verapamil, cepharanthine, and γ-oryzanol; skin astringents such as zinc oxide and tannic acid; and antiseborrheic agents such as sulfur and thianthrol.
[0106] Vitamins: Vitamins include vitamin A oil, retinol, retinol acetate, retinol palmitate, and other vitamin A derivatives, riboflavin, riboflavin butyrate, flavin adenine nucleotide, and other vitamin B2 derivatives, pyridoxine hydrochloride, pyridoxine dioctanoate, pyridoxine tripalmitate, and other vitamin B6 derivatives, vitamin B12 and its derivatives, vitamin B15 and its derivatives, L-ascorbic acid, L-ascorbic acid dipalmitate, sodium L-ascorbic acid-2-sulfate, and dipotassium L-ascorbic acid phosphate diester. vitamin C such as ergocalciferol and cholecalciferol; vitamin D such as α-tocopherol, β-tocopherol, γ-tocopherol, dl-α-tocopherol acetate, dl-α-tocopherol nicotinate, and dl-α-tocopherol succinate; nicotinic acids such as nicotinic acid, benzyl nicotinate, and nicotinamide; vitamin H, vitamin P, pantothenic acids such as calcium pantothenate, D-pantothenyl alcohol, pantothenyl ethyl ether, and acetylpantothenyl ethyl ether; and biotin.
[0107] Amino acids include glycine, valine, leucine, isoleucine, serine, threonine, phenylalanine, arginine, lysine, aspartic acid, glutamic acid, cystine, cysteine, methionine, and tryptophan.
[0108] Nucleic Acids Examples of nucleic acids include deoxyribonucleic acid.
[0109] Hormones include estradiol and ethenylestradiol.
[0110] Inclusion Compounds Examples of inclusion compounds include cyclodextrin.
[0111] The present invention is applicable to various types of cosmetics, but particularly preferred are cosmetics applied to the skin, such as skin care cosmetics, makeup cosmetics, antiperspirant cosmetics, and UV protection cosmetics, cosmetics applied to the hair, such as hair cosmetics, and nail cosmetics. Examples of skin care cosmetics include lotions, emulsions, creams, cleansers, face packs, oil liquids, massage products, beauty serums, beauty oils, detergents, deodorants, hand creams, lip balms, and wrinkle concealers. Examples of makeup cosmetics include makeup bases, foundations, concealers, face powders, blushers, eyeshadows, eyeshadows, mascaras, eyeliners, eyebrow pencils, and lipsticks. Examples of antiperspirant cosmetics include roll-on, cream, solution, and stick-type antiperspirant cosmetics. Examples of UV protection cosmetics include sunscreen oils, sunscreen emulsions, and sunscreen creams. Examples of hair cosmetics include shampoos, conditioners, treatments, and setting agents.
[0112] The cosmetic of the present invention may be in any form, for example, a powder, an oily liquid, a water-in-oil emulsion, an oil-in-water emulsion, a non-aqueous emulsion, or a multiple emulsion such as a W / O / W type or an O / W / O type. The cosmetic of the present invention may be in any form, such as a liquid, emulsion, cream, solid, paste, gel, powder, pressed, multi-layered, mousse, spray, stick, or pencil.
[0113] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the following examples, unless otherwise specified, "%" in the composition is % by mass, and the blend amount is the blend amount of the blended product described.
[0114] Example 1 50 g of triglycerin diallyl ether represented by the following formula (E-1), 128.7 g of organohydrogenpolysiloxane represented by the following formula (E-2) (hydrosilyl group / allyl group = 2.0 / 2.0 [molar ratio]), 89.3 g of isopropyl alcohol, and 0.04 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were charged into a reactor and heated at 80°C for 5 hours to carry out a reaction. Subsequently, 15.4 g of 0.01 N (mol / L) hydrochloric acid was added, and the mixture was heated at 80°C for 3 hours to carry out hydrolysis, followed by neutralization with 0.2 g of 5% aqueous sodium bicarbonate. The reaction solution was heated under reduced pressure to distill off the solvent, and the filtrate was filtered to obtain the target product (organopolysiloxane), which was a fluid, viscous liquid represented by the following formula (E-3).
[0115] Example 2 50 g of triglycerin diallyl ether represented by formula (E-1) above, 244.8 g of organohydrogenpolysiloxane represented by formula (E-4) below (hydrosilyl group / allyl group = 2.0 / 2.0 [molar ratio]), 88.4 g of isopropyl alcohol, and 0.03 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were charged into a reactor and heated at 80°C for 5 hours to carry out a reaction. Subsequently, 29.4 g of 0.01 N hydrochloric acid was added, and the mixture was heated at 80°C for 3 hours to carry out hydrolysis, followed by neutralization with 0.4 g of 5% aqueous sodium bicarbonate. The reaction solution was heated under reduced pressure to distill off the solvent, and the filtrate was filtered to obtain the target product (organopolysiloxane), which was a fluid, viscous liquid represented by formula (E-5) below.
[0116] Example 3 50 g of triglycerin diallyl ether represented by the formula (E-1), 729.2 g of organohydrogenpolysiloxane represented by the following formula (E-6) (hydrosilyl group / allyl group = 1.0 / 2.0 [molar ratio]), 389.6 g of isopropyl alcohol, and 0.16 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were charged into a reactor and reacted by heating for 5 hours at 80 ° C. Thereafter, 122.4 g of organohydrogenpolysiloxane represented by the formula (E-4) (hydrosilyl group / allyl group = 1.0 / 2.0 [molar ratio]), 61.2 g of isopropyl alcohol, and 0.02 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were charged into a reactor and reacted by heating for 3 hours at 80 ° C. Subsequently, 102.2 g of 0.01 N hydrochloric acid was added and the mixture was heated at 80°C for 3 hours to carry out hydrolysis, followed by neutralization with 1.5 g of 5% aqueous sodium bicarbonate. The reaction solution was heated under reduced pressure to distill off the solvent, and the filtrate was filtered to obtain the target product (organopolysiloxane) which was a fluid viscous liquid represented by the following formula (E-7):
[0117] Example 4 50 g of diglycerin diallyl ether represented by the following formula (E-8), 248.8 g of organohydrogenpolysiloxane represented by the following formula (E-9) (hydrosilyl group / allyl group=1.0 / 2.0 [molar ratio]), 119.5 g of isopropyl alcohol, and 0.07 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were placed in a reactor, and the mixture was heated at 80° C. for 5 hours to carry out a reaction. Thereafter, 30.1 g of an organohydrogenpolysiloxane represented by the following formula (E-10) (hydrosilyl group / allyl group = 1.0 / 2.0 [molar ratio]), 12.0 g of isopropyl alcohol, and 0.01 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were charged into a reactor and heated at 80°C for 3 hours to carry out a reaction. Subsequently, 33.5 g of 0.01 N hydrochloric acid was added and the mixture was heated at 80°C for 3 hours to carry out hydrolysis, followed by neutralization with 0.5 g of 5% aqueous sodium bicarbonate. The reaction solution was heated under reduced pressure to distill off the solvent, and the mixture was filtered to obtain the target product (organopolysiloxane), which was a fluid, viscous liquid represented by the following formula (E-11).
[0118] Example 5 50 g of pentaglycerin triallyl ether represented by the following formula (E-12), 330.4 g of organohydrogenpolysiloxane represented by the following formula (E-13) (hydrosilyl group / allyl group=2.0 / 3.0 [molar ratio]), 304.3 g of isopropyl alcohol, and 0.13 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were placed in a reactor, and the mixture was heated at 80° C. for 5 hours to carry out a reaction. Thereafter, 36.6 g of the organohydrogenpolysiloxane represented by the formula (E-14) (hydrosilyl group / allyl group = 1.0 / 3.0 [molar ratio]), 29.3 g of isopropyl alcohol, and 0.01 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were charged into a reactor and heated at 80°C for 3 hours to carry out a reaction. Subsequently, 44.0 g of 0.01 N hydrochloric acid was added and the mixture was heated at 80°C for 3 hours to carry out hydrolysis, followed by neutralization with 0.7 g of 5% aqueous sodium bicarbonate. The reaction solution was heated under reduced pressure to distill off the solvent, and the mixture was filtered to obtain the target product (organopolysiloxane), which was a fluid, viscous liquid represented by the following formula (E-15).
[0119] Example 6 50 g of tetraglycerin dioctenyl ether represented by the following formula (E-16), 566.9 g of organohydrogenpolysiloxane represented by the following formula (E-17) (hydrosilyl group / octenyl group=1.0 / 2.0 [molar ratio]), 370.1 g of isopropyl alcohol, and 0.10 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were placed in a reactor, and the mixture was heated at 80° C. for 5 hours to carry out a reaction. Thereafter, 61.7 g of an organohydrogenpolysiloxane represented by the following formula (E-18) (hydrosilyl group / allyl group = 1.0 / 2.0 [molar ratio]), 37.0 g of isopropyl alcohol, and 0.01 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were charged into a reactor and heated at 80°C for 3 hours to carry out a reaction. Subsequently, 75.4 g of 0.01 N hydrochloric acid was added, and the mixture was heated at 80°C for 3 hours to carry out hydrolysis, followed by neutralization with 1.1 g of 5% aqueous sodium bicarbonate. The reaction solution was heated under reduced pressure to distill off the solvent, and the resulting mixture was filtered to obtain the target product (organopolysiloxane), which was a fluid, viscous liquid represented by the following formula (E-19).
[0120] Example 7 50 g of tetraglycerin triallyl ether represented by the following formula (E-20), 730.3 g of organohydrogenpolysiloxane represented by the following formula (E-21) (hydrosilyl group / allyl group=2.0 / 3.0 [molar ratio]), 234.1 g of isopropyl alcohol, and 0.13 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were placed in a reactor, and the mixture was heated at 80° C. for 5 hours to carry out a reaction. Thereafter, 82.0 g of an organohydrogenpolysiloxane represented by the following formula (E-22) (hydrosilyl group / allyl group=1.0 / 3.0 [molar ratio]), 24.6 g of isopropyl alcohol, and 0.01 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were charged into a reactor and heated at 80°C for 3 hours to carry out a reaction. Subsequently, 97.5 g of 0.01 N hydrochloric acid was added, and the mixture was heated at 80°C for 3 hours to carry out hydrolysis, followed by neutralization with 1.5 g of 5% aqueous sodium bicarbonate. The reaction solution was heated under reduced pressure to distill off the solvent, and the resulting mixture was filtered to obtain the target product (organopolysiloxane), which was a fluid, viscous liquid represented by the following formula (E-23).
[0121] Example 8 50 g of triglycerin dioctenyl ether represented by the following formula (E-24), 1739.1 g of organohydrogenpolysiloxane represented by the following formula (E-25) (hydrosilyl group / octenyl group=1.0 / 2.0 [molar ratio]), 447.3 g of isopropyl alcohol, and 0.24 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were placed in a reactor, and the mixture was heated at 80° C. for 5 hours to carry out a reaction. Thereafter, 52.8 g of an organohydrogenpolysiloxane represented by the following formula (E-26) (hydrosilyl group / allyl group=1.0 / 2.0 [molar ratio]), 13.2 g of isopropyl alcohol, and 0.01 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were charged into a reactor and heated at 80°C for 3 hours to carry out a reaction. Subsequently, 215.0 g of 0.01 N hydrochloric acid was added, and the mixture was heated at 80°C for 3 hours to carry out hydrolysis, followed by neutralization with 3.2 g of 5% aqueous sodium bicarbonate. The reaction solution was heated under reduced pressure to distill off the solvent, and the resulting mixture was filtered to obtain the target product (organopolysiloxane), which was a fluid, viscous liquid represented by the following formula (E-27).
[0122] Example 9 50 g of tetraglycerin diallyl ether represented by the following formula (E-28), 710.7 g of organohydrogenpolysiloxane represented by the following formula (E-29) (hydrosilyl group / allyl group=1.0 / 2.0 [molar ratio]), 532.5 g of isopropyl alcohol, and 0.15 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were placed in a reactor, and the mixture was heated at 80° C. for 5 hours to carry out a reaction. Thereafter, 71.1 g of an organohydrogenpolysiloxane represented by the following formula (E-30) (hydrosilyl group / allyl group = 1.0 / 2.0 [molar ratio]), 49.8 g of isopropyl alcohol, and 0.01 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were charged into a reactor and heated at 80°C for 3 hours to carry out a reaction. Subsequently, 93.8 g of 0.01 N hydrochloric acid was added, and the mixture was heated at 80°C for 3 hours to carry out hydrolysis, followed by neutralization with 1.4 g of 5% aqueous sodium bicarbonate. The reaction solution was heated under reduced pressure to distill off the solvent, and the resulting mixture was filtered to obtain the target product (organopolysiloxane), which was a fluid, viscous liquid represented by the following formula (E-31).
[0123] Example 10 50 g of pentaglycerin triallyl ether represented by the following formula (E-12), 603.4 g of organohydrogenpolysiloxane represented by the following formula (E-32) (hydrosilyl group / allyl group=2.0 / 3.0 [molar ratio]), 261.4 g of isopropyl alcohol, and 0.22 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were placed in a reactor, and the mixture was heated at 80° C. for 5 hours to carry out a reaction. Thereafter, 56.8 g of an organohydrogenpolysiloxane represented by the following formula (E-33) (hydrosilyl group / allyl group = 1.0 / 3.0 [molar ratio]), 22.7 g of isopropyl alcohol, and 0.02 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were charged into a reactor and heated at 80°C for 3 hours to carry out a reaction. Subsequently, 79.2 g of 0.01 N hydrochloric acid was added, and the mixture was heated at 80°C for 3 hours to carry out hydrolysis, followed by neutralization with 1.2 g of 5% aqueous sodium bicarbonate. The reaction solution was heated under reduced pressure to distill off the solvent, and the resulting mixture was filtered to obtain the target product (organopolysiloxane), which was a fluid, viscous liquid represented by the following formula (E-34).
[0124] Comparative Example 1 50 g of triglycerin diallyl ether represented by the formula (E-1) above, 1,060.6 g of organohydrogenpolysiloxane represented by the following formula (E-35) (hydrosilyl group / allyl group=1.0 / 2.0 [molar ratio]), 333.2 g of isopropyl alcohol, and 0.19 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were placed in a reactor, and the mixture was heated at 80° C. for 5 hours to carry out a reaction. Thereafter, 376.3 g of an organohydrogenpolysiloxane represented by the following formula (E-36) (hydrosilyl group / allyl group=1.0 / 2.0 [molar ratio]), 112.9 g of isopropyl alcohol, and 0.06 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were charged into a reactor and heated at 80°C for 3 hours to carry out a reaction. Subsequently, 172.4 g of 0.01 N hydrochloric acid was added, and the mixture was heated at 80°C for 3 hours to carry out hydrolysis, followed by neutralization with 2.6 g of 5% aqueous sodium bicarbonate. The reaction solution was heated under reduced pressure to distill off the solvent, and the resulting mixture was filtered to obtain the target product (organopolysiloxane), which was a fluid, viscous liquid represented by the following formula (E-37).
[0125] Comparative Example 2 50 g of triglycerin diallyl ether represented by the formula (E-1), 1458.3 g of organohydrogenpolysiloxane represented by the formula (E-6) (hydrosilyl group / allyl group = 2.0 / 2.0 [molar ratio]), 905.0 g of isopropyl alcohol, and 0.30 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were charged into a reactor and heated at 80°C for 5 hours to carry out a reaction. Subsequently, 183.2 g of 0.01 N hydrochloric acid was added and the mixture was heated at 80°C for 3 hours to carry out hydrolysis, followed by neutralization with 2.8 g of 5% aqueous sodium bicarbonate. The reaction solution was heated under reduced pressure to distill off the solvent, and the mixture was filtered to obtain the target product, a fluid viscous liquid represented by the following formula (E-38).
[0126] Comparative Example 3 50 g of tetraglycerin diallyl ether represented by the formula (E-28) above, 1,895.1 g of an organohydrogenpolysiloxane represented by the following formula (E-39) (hydrosilyl group / allyl group = 2.0 / 2.0 [molar ratio]), 972.5 g of isopropyl alcohol, and 0.20 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were charged into a reactor and heated at 80°C for 5 hours to carry out a reaction. Subsequently, 234.1 g of 0.01 N hydrochloric acid was added, and the mixture was heated at 80°C for 3 hours to carry out hydrolysis, followed by neutralization with 3.5 g of 5% aqueous sodium bicarbonate. The reaction solution was heated under reduced pressure to distill off the solvent, and the filtrate was filtered to obtain the target product (organopolysiloxane), which was a fluid, viscous liquid represented by the following formula (E-40).
[0127] Comparative Example 4 50 g of triglycerin diallyl ether represented by the formula (E-1) above, 1891.9 g of an organohydrogenpolysiloxane represented by the following formula (E-41) (hydrosilyl group / allyl group = 2.0 / 2.0 [molar ratio]), 776.8 g of isopropyl alcohol, and 0.65 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were charged into a reactor and heated at 80°C for 5 hours to carry out a reaction. Subsequently, 235.3 g of 0.01 N hydrochloric acid was added and the mixture was heated at 80°C for 3 hours to carry out hydrolysis, followed by neutralization with 3.5 g of 5% aqueous sodium bicarbonate. The reaction solution was heated under reduced pressure to distill off the solvent, and the filtrate was filtered to obtain the target product (organopolysiloxane), which was a fluid, viscous liquid represented by the following formula (E-42).
[0128] Comparative Example 5 50 g of pentaglycerin triallyl ether represented by the following formula (E-12), 797.6 g of organohydrogenpolysiloxane represented by the above formula (E-17) (hydrosilyl group / allyl group=2.0 / 3.0 [molar ratio]), 762.9 g of isopropyl alcohol, and 0.23 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were placed in a reactor, and the mixture was heated at 80° C. for 5 hours to carry out a reaction. Thereafter, 110.1 g of an organohydrogenpolysiloxane represented by the following formula (E-43) (hydrosilyl group / allyl group = 1.0 / 3.0 [molar ratio]), 99.1 g of isopropyl alcohol, and 0.03 g of a 3% ethanol solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex were charged into a reactor and heated at 80°C for 3 hours to carry out a reaction. Subsequently, 108.9 g of 0.01 N hydrochloric acid was added, and the mixture was heated at 80°C for 3 hours to carry out hydrolysis, followed by neutralization with 1.6 g of 5% aqueous sodium bicarbonate. The reaction solution was heated under reduced pressure to distill off the solvent, and the mixture was filtered to obtain the target product (organopolysiloxane), which was a fluid, viscous liquid represented by the following formula (E-44).
[0129] The present invention will be specifically explained below with reference to formulation examples of cosmetic compositions and comparative examples, but the present invention is not limited to these examples. The average particle size in the tables is the "average primary particle size."
[0130] [Examples 11 to 12, Comparative Examples 6 to 10] Oily pastes were prepared according to the formulations shown in Table 1. (Production Method) A: Component (1) was dispersed using a roll to obtain a paste-like dispersion.
[0131] [Processing step: Dispersibility] In the process A, those which were good in dispersibility and easy to roll process were marked with "◯", and those which were poor in dispersibility and difficult to roll process were marked with "X".
[0132] [Hardness Stability] When the hardness of the obtained paste was compared on the day and after one week at 25°C, a change of less than 150% was marked as "◎", a change of 150% or more but less than 200% was marked as "○", and a poor stability of 200% or more was marked as "×". Pastes with insufficient treatment steps were not evaluated. The hardness was measured using a rheometer RT-2002D-D (manufactured by Rheotec Corporation, measuring probe: 10 mmφ, penetration depth: 10 mm, sample stage rising speed: 5 cm / min, temperature: 25°C, range: 200).
[0133] KF-96A-6cs: Shin-Etsu Chemical
[0134] The results in Table 1 above show that the organopolysiloxane of the present invention has excellent dispersibility and can be used to prepare pastes with lower viscosity. The improved dispersibility of the paste allows for greater freedom in formulation, and the dispersion stability is also excellent.
[0135] [Example 13, Comparative Examples 11 to 15] Dispersions were prepared according to the formulations shown in Table 2. (Production Method) A: Zirconia beads were added to component (1), and the mixture was dispersed using a paint shaker to obtain a dispersion.
[0136] [Initial Viscosity] The viscosity of the obtained dispersion was measured at 25°C immediately after preparation. The viscosity was measured using a Brookfield viscometer with a spindle LV-2 at 30 revolutions per minute after 60 seconds. The unit is mPa s. A viscosity exceeding the upper limit of measurement, 1,000 mPa s, was marked "X." Viscosities within the range that can be measured under these conditions are low viscosity and easy to handle.
[0137] [Viscosity stability] When the viscosity of the obtained dispersion was compared on the day of measurement and after one week at 25°C, a change of less than 150% was marked as "◎", a change of less than 200% was marked as "○", and a change of 200% or more due to poor stability was marked as "×". Viscosity values exceeding the upper limit of viscosity measurement were not evaluated.
[0138] KF-96L-2cs (Dimethicone): Shin-Etsu Chemical Co., Ltd. (hereinafter the same)
[0139] The results in Table 2 above show that the organopolysiloxane of the present invention has excellent dispersibility and can be used to prepare dispersions with lower viscosities. This improves the dispersibility of the dispersion, increasing the degree of freedom in formulation and providing favorable dispersion stability.
[0140] [Examples 14 to 15, Comparative Examples 16 to 20] Dispersions were prepared according to the formulations shown in Table 3. (Production Method) A: Zirconia beads were filled into component (1), and the mixture was dispersed using a paint shaker to obtain a dispersion.
[0141] [Initial Viscosity] The viscosity of the resulting dispersion was measured immediately after preparation. The viscosity was measured using a Brookfield viscometer with a spindle LV-2 at 30 revolutions per minute for 60 seconds. The unit is mPa s. Values exceeding the upper limit of measurement, 1,000 mPa s, were marked "x." Viscosities within the range that can be measured under these conditions are low and easy to handle.
[0142] [Viscosity stability] When the viscosity of the obtained dispersion was compared on the day of measurement and after one week at 25°C, a change of less than 150% was marked as "◎", a change of less than 200% was marked as "○", and a change of 200% or more due to poor stability was marked as "×". Viscosity values exceeding the upper limit of measurement were not evaluated.
[0143]
[0144] [Example 16, Comparative Examples 21 to 25] Dispersions were prepared according to the formulations shown in Table 4. (Production Method) A: Zirconia beads were added to component (1), and the mixture was dispersed using a paint shaker to obtain a dispersion.
[0145] [Initial Viscosity] The viscosity of the obtained dispersion was measured at 25°C immediately after preparation. The viscosity was measured using a Brookfield viscometer with a spindle LV-2 at 30 revolutions per minute after 60 seconds. The unit is mPa s. A viscosity exceeding the upper limit of measurement, 1,000 mPa s, was marked "X." Viscosities within the range that can be measured under these conditions are low viscosity and easy to handle.
[0146] [Viscosity stability] When the viscosity of the obtained dispersion was compared on the day of measurement and after one week at 25°C, a change of less than 150% was marked as "◎", a change of less than 200% was marked as "○", and a change of 200% or more due to poor stability was marked as "×". Viscosity values exceeding the upper limit of measurement were not evaluated.
[0147]
[0148] The results in Table 4 above show that the organopolysiloxane of the present invention has excellent dispersibility and can prepare dispersions with lower viscosity. The dispersibility of the dispersion is improved, which increases the degree of freedom in formulation, and the viscosity and dispersion stability of the powder are favorable.
[0149] [Examples 17 to 20, Comparative Examples 26 to 30] Emulsion cosmetics were prepared according to the formulations shown in Table 5. (Production Method) A: Component (2) was added to component (1) and emulsified to obtain a cream.
[0150] [Usage sensation] A panel of 10 experts applied each sample (cream) to the cheeks and evaluated the stickiness upon application sensorily. The evaluation criteria were 5 points if almost no stickiness was felt, 3 points if slight stickiness was felt, and 1 point if stickiness was felt, and the total score was calculated. ◎: Total score of 45 points or more ○: Total score of 40 to 44 points △: Total score of 21 to 39 points ×: Total score of 20 points or less A score of "○" or higher was considered a pass.
[0151] [Spreadability] A panel of experts (10 people) applied each sample (cream) to the cheeks and evaluated sensory assessment of how well it spread when applied. The evaluation criteria were 5 points for good spreadability, 3 points for slightly poor spreadability, and 1 point for poor spreadability, and the total points were calculated. ◎: Total point is 45 points or more ○: Total point is 40 to 44 points △: Total point is 21 to 39 points ×: Total point is 20 points or less A score of "○" or higher was considered a pass.
[0152]
[0153] The results in Table 5 above demonstrate that the organopolysiloxane of the present invention is excellent in feel and spreadability.
[0154] Example 21 Oil-in-Water Sunscreen Cream Composition % 1. Organopolysiloxane of Example 3 0.5 2. Silicone-treated zinc oxide microparticles 5 3. Decamethylcyclopentasiloxane 5 4. Ethylhexyl methoxycinnamate 5 5. KF-56A (Note 1) 3 6. Cetyl alcohol 0.5 7. Polyoxyethylene sorbitan monooleate 2.5 8. Glyceryl stearate (SE) 0.5 9. KF-6011P (Note 2) 1 10. Dipropylene glycol 6 11. 1,3-butylene glycol 6 12. Carboxyvinyl polymer 0.3 13. Acrylic polymer 0.3 14. Methylparaben 0.2 15. Phenoxyethanol 0.3 16. Disodium edetate (as needed) 17. Water (remaining amount) 18. 10% aqueous sodium hydroxide solution (as needed) Total 100.0 (Note 1) Shin-Etsu Chemical Co., Ltd.: Diphenylsiloxyphenyl trimethicone (Note 2) Shin-Etsu Chemical Co., Ltd.: PEG-11 methyl ether dimethicone
[0155] (Production Method) A: Components 1 to 3 were mixed uniformly in a bead mill. B: The mixture obtained in A and 4 to 6 were mixed uniformly at 90°C. C: Components 7 to 17 were mixed uniformly at 85°C. D: The mixture obtained in B was added to the mixture obtained in C and emulsified, and component 18 was added and mixed uniformly to obtain an O / W sunscreen. The obtained O / W sunscreen had high transparency, little stickiness, and a good feel when used.
[0156] [Example 22] W / O Cream Composition % 1. KSG-710 (Note 1) 4 2. KSG-15 (Note 2) 1 3. Organopolysiloxane of Example 5 3 4. Dimethylpolysiloxane (6cs) 13 5. 1,3-butylene glycol 8 6. Sorbitol 5 7. Phenoxyethanol 0.3 8. Sodium citrate appropriate amount 9. Sodium chloride appropriate amount 10. Water Remaining volume Total 100.0 (Note 1) Shin-Etsu Chemical Co., Ltd.: Mixture of 70-80% dimethicone + 20-30% (dimethicone / polyglycerin-3) crosspolymer (Note 2) Shin-Etsu Chemical Co., Ltd.: Mixture of 90-96% cyclopentasiloxane + 4-10% (dimethicone / vinyl dimethicone) crosspolymer
[0157] (Production method) A: Components 1 to 4 were mixed uniformly. B: Components 5 to 10 were mixed uniformly. C: The mixture obtained in B was added to the mixture obtained in A and emulsified to obtain a W / O cream. The obtained W / O cream had a moisturizing feel, was not sticky, and had a good feel when used.
[0158] Example 23 W / O Shaking Sunscreen Composition % 1. Organopolysiloxane of Example 1 2.8 2. Organopolysiloxane of Example 6 1.7 3. Metal soap-treated fine particle titanium dioxide 14 4. Hydrogen dimethicone-treated fine particle zinc oxide 21 5. Decamethylcyclopentasiloxane 12 6. Decamethylcyclopentasiloxane 12 7. KSG-15 (Note 1) 2 8. KSG-16 (Note 2) 4 9. KF-6104 (Note 3) 0.5 10. Decamethylcyclopentasiloxane balance 11. Dimethylpolysiloxane (6cs) 3 12. Isotridecyl isononanoate 4.8 13. KSP-105 (Note 4) 1 14. 1,3-butylene glycol 2 15. Phenoxyethanol Appropriate amount 16. Sodium citrate Appropriate amount 17. Sodium chloride Appropriate amount 18. Purified water 13 Total 100.0 (Note 1) Shin-Etsu Chemical Co., Ltd.: Cyclopentasiloxane 90-96% + (Dimethicone / Vinyl Dimethicone) Crosspolymer 4-10% Mixture (Note 2) Shin-Etsu Chemical Co., Ltd.: Dimethicone 70-80% + (Dimethicone / Vinyl Dimethicone) Crosspolymer 20-30% Mixture (Note 3) Shin-Etsu Chemical Co., Ltd.: Polyglyceryl-3 Polydimethylsiloxyethyl Dimethicone (Note 4) Shin-Etsu Chemical Co., Ltd.: (Vinyl Dimethicone / Methicone Silsesquioxane) Crosspolymer
[0159] (Production Method) A: Components 1, 3, and 5 were mixed uniformly using a homomixer. B: Components 2, 4, and 6 were mixed uniformly using a homomixer. C: The mixture obtained in A, the mixture obtained in B, and components 7 to 12 were mixed uniformly. D: Components 13 to 18 were mixed uniformly. E: The mixture obtained in D was added to the mixture obtained in C and emulsified to obtain a W / O shaking sunscreen. The obtained W / O shaking sunscreen contained a high blend of fine particle powder, but had low viscosity, high transparency, was non-sticky, and had a good feel when used. In addition, viscosity increase at high temperatures was suppressed, and it had excellent stability.
[0160] Example 24 W / O Liquid Foundation Composition % 1. KSG-210 (Note 1) 3 2. KSG-44 (Note 2) 7 3. KF-6028 (Note 3) 2 4. KF-6038 (Note 4) 1 5. Trisiloxane balance 6. Organically modified clay mineral 1 7. Organopolysiloxane of Example 7 1 8. Dimethylpolysiloxane (6cs) 5 9. Isotridecyl isononanoate 7 10. KTP-09W (Note 5) 8.5 11. KTP-09Y (Note 5) 1 12. KTP-09R (Note 5) 0.4 13. KTP-09B (Note 5) 0.1 14. Metal soap-treated titanium oxide microparticles 5 15. Dipropylene glycol 5 16. Phenoxyethanol 0.2 17. Sodium citrate appropriate amount 18. Magnesium sulfate appropriate amount 19. Water 33 Total 100.0 (Note 1) Shin-Etsu Chemical Co., Ltd.: Dimethicone 70-80% + (Dimethicone / (PEG-10 / 15)) Crosspolymer 20-30% Mixture (Note 2) Shin-Etsu Chemical Co., Ltd.: Squalane 65-75% + (Vinyl Dimethicone / Lauryl Dimethicone) Crosspolymer 25-35% Mixture (Note 3) Shin-Etsu Chemical Co., Ltd.: PEG-9 Polydimethylsiloxyethyl Dimethicone (Note 4) Shin-Etsu Chemical Co., Ltd.: Lauryl PEG-9 Polydimethylsiloxyethyl Dimethicone (Note 5) Shin-Etsu Chemical Co., Ltd.: KF-9909 treated colored inorganic pigment, W: White, R: Red, Y: Yellow, B: Black
[0161] (Production method) A: Components 7 to 14 were made into a paste using a three-roll mill. B: The mixture obtained in A and components 1 to 6 were mixed uniformly. C: Components 15 to 19 were mixed uniformly. D: The mixture obtained in C was added to the mixture obtained in B and emulsified to obtain a W / O liquid foundation. The obtained W / O liquid foundation contained a high powder content, but had low viscosity, good spreadability, and a good feel when used. In addition, viscosity increase at high temperatures was suppressed, providing excellent stability.
[0162] Example 25 W / O Cream Foundation Composition % 1. KSG-270 (Note 1) 3 2. KSG-18A (Note 2) 7 3. KF-6038 (Note 3) 3 4. Hydrogenated farnesene balance 5. Ethylhexyl triazone 4 6. Diethylamino hydroxybenzoyl hexyl benzoate 1 7. Organically modified clay mineral 1.2 8. Organopolysiloxane of Example 8 1.5 9. KF-56A (Note 4) 10 10. Coco-caprylate / caprate 7 11. KTP-09W (Note 5) 8.5 12. KTP-09Y (Note 5) 1 13. KTP-09R (Note 5) 0.4 14. KTP-09B (Note 5) 0.1 15. Metal soap-treated titanium dioxide fine particle 10 16. Dipropylene glycol 5 17. Phenoxyethanol 0.2 18. Sodium citrate appropriate amount 19. Magnesium sulfate appropriate amount 20. Purified water 30 Total 100.0 (Note 1) Shin-Etsu Chemical Co., Ltd.: Mixture of 75-85% diphenylsiloxyphenyl trimethicone + 15-25% (dimethicone / (PEG-10 / 15)) crosspolymer (Note 2) Shin-Etsu Chemical Co., Ltd.: Mixture of 80-90% diphenylsiloxyphenyl trimethicone + 10-20% (dimethicone / phenylvinyl dimethicone) crosspolymer (Note 3) Shin-Etsu Chemical Co., Ltd.: Lauryl PEG-9 polydimethylsiloxyethyl dimethicone (Note 4) Shin-Etsu Chemical Co., Ltd.: Diphenylsiloxyphenyl trimethicone(Note 5) Shin-Etsu Chemical Co., Ltd.: KF-9909 treated colored inorganic pigment, W: white, R: red, Y: yellow, B: black
[0163] (Production method) A: Components 8 to 15 were made into a paste using a triple roll. B: The mixture obtained in A and components 1 to 7 were mixed uniformly. C: Components 16 to 20 were mixed uniformly. D: The mixture obtained in C was added to the mixture obtained in B and emulsified to obtain a W / O cream foundation. The obtained W / O cream foundation had a high powder content, but spread well and felt good in use.
[0164] [Example 26] Non-aqueous concealer Composition % 1. KSP-101 (Note 1) 23 2. KSP-300 (Note 2) 5 3. KSG-19 (Note 3) 6 4. Dimethylpolysiloxane (6cs) 40 5. KF-56A (Note 4) 7 6. TMF-1.5 (Note 5) balance 7. Triethylhexanoin 0.2 8. Organopolysiloxane from Example 9 0.5 9. AES-3083-treated titanium dioxide (Note 6) 0.3 10. AES-3083 treated iron oxide (Note 6) Appropriate amount Total 100.0 (Note 1) Shin-Etsu Chemical Co., Ltd.: (Vinyl dimethicone / methicone silsesquioxane) crosspolymer (Note 2) Shin-Etsu Chemical Co., Ltd.: (Diphenyl dimethicone / vinyl diphenyl dimethicone / silsesquioxane) crosspolymer (Note 3) Shin-Etsu Chemical Co., Ltd.: Mixture of 80-90% dimethicone + 10-20% (dimethicone / vinyl dimethicone) crosspolymer (Note 4) Shin-Etsu Chemical Co., Ltd.: Diphenylsiloxyphenyl trimethicone (Note 5) Shin-Etsu Chemical Co., Ltd.: Methyl trimethicone (Note 6) Shin-Etsu Chemical Co., Ltd.: Triethoxycaprylylsilane treated colored inorganic pigment
[0165] (Production method) A: Components 7 to 10 were prepared into a paste using a disper. B: The mixture obtained in A and components 1 to 6 were mixed uniformly to obtain a non-aqueous concealer. The obtained non-aqueous concealer had good powder dispersibility and was also pleasant to use.
[0166] Example 27 Lipstick Composition % 1. Candelilla wax 3 2. Polyethylene 2 3. Microcrystalline wax 2.5 4. Ceresin 6 5. KP-561P (Note 1) 13 6. Macadamia nut oil 23 7. Diisostearyl malate 8.5 8. Hydrogenated polyisobutene 8.5 9. Isotridecyl isononanoate 15 10. Polyglyceryl-2 triisostearate 4.5 11. Organopolysiloxane of Example 10 2.5 12. Red No. 201 0.4 13. Red No. 202 0.4 14. Yellow No. 4 1.6 15. KTP-09W (Note 2) 3 16. KTP-09R (Note 2) 0.7 17. KTP-09B (Note 2) 0.2 18. KF-9909 treated (Note 3) talc 0.719. Mica 4.5 Total 100.0 (Note 1) Shin-Etsu Chemical Co., Ltd.: (Acrylates / stearyl acrylate / dimethicone methacrylate) copolymer (Note 2) Shin-Etsu Chemical Co., Ltd.: KF-9909 treated colored inorganic pigment, W: white, R: red, B: black (Note 3) Shin-Etsu Chemical Co., Ltd.: triethoxysilylethyl polydimethylsiloxyethylhexyl dimethicone
[0167] (Production Method) A: Components 10 to 18 were dispersed using a roll mill. B: Components 1 to 9 were mixed uniformly at 90°C. C: The mixture obtained in A and component 19 were added to the mixture obtained in B, mixed uniformly at 80°C, filled into a mold, and slowly cooled to obtain a lipstick. The obtained lipstick had excellent adhesion and a good feel when used. This demonstrates that the product can also be used in other non-aqueous oil-based cosmetics such as glosses, stick concealers, and pour-on foundations.
[0168] Example 28 W / O Solid Foundation Composition % 1. KSG-710 (Note 1) 5 2. KSG-19 (Note 2) 3 3. Organopolysiloxane of Example 3 2 4. SPD-Z7L (Note 3) 10 5. KF-56A (Note 4) 7.35 6. Ceresin 5 7. Octyldodecyl myristate 2 8. KF-9901-treated titanium dioxide (Note 5) 7 9. KF-9901-treated black iron oxide (Note 5) 0.1 10. KF-9901-treated red iron oxide (Note 5) 0.3 11. KF-9901-treated yellow iron oxide (Note 5) 0.6 12. KP-549 (Note 6) 0.3 13. BG 7 14. Glycerin 5 15. Sodium citrate 0.2 16. Sodium chloride 117. Water Remaining volume Total 100.0 (Note 1) Shin-Etsu Chemical Co., Ltd.: Dimethicone (6cs) 70-80% + (Dimethicone / Polyglycerin-3) Crosspolymer 20-30% mixture (Note 2) Shin-Etsu Chemical Co., Ltd.: Dimethicone (6cs) 80-90% + (Dimethicone / Vinyl Dimethicone) Crosspolymer 10-20% mixture (Note 3) Shin-Etsu Chemical Co., Ltd.: Dimethicone (2cs) dispersion of 60% fine zinc oxide (Note 4) Shin-Etsu Chemical Co., Ltd.: Diphenylsiloxyphenyl trimethicone (Note 5) Shin-Etsu Chemical Co., Ltd.: Hydrogen dimethicone-treated colored inorganic pigment (Note 6) Shin-Etsu Chemical Co., Ltd.: (Acrylates / Dimethicone) Copolymer
[0169] (Production Method) A: Components 7 to 12 were dispersed using a high-pressure disperser. B: Components 1 to 6 were dissolved at 90°C, and the mixture obtained in A was added and mixed uniformly. C: Components 13 to 17 were mixed uniformly. D: The mixture obtained in C was added to the mixture obtained in B and emulsified to obtain a W / O solid foundation. The obtained W / O solid foundation had a good feel when used, good application properties, and excellent storage stability.
[0170] [Example 29] Lipstick Composition % 1. Synthetic wax 6 2. Paraffin 6 3. Microcrystalline wax 2 4. Organopolysiloxane of Example 9 2.5 5. KF-56A (Note 1) 5 6. Dipentaerythrityl tri-polyhydroxystearate balance 7. Jojoba seed oil 1.5 8. Hydrogenated polyisobutene 12 9. Di(phytosteryl / octyldodecyl) lauroyl glutamate 1.5 10. Organopolysiloxane of Example 10 3 11. Triethylhexanoin 15 12. Tri(caprylic / capric)glyceryl 7 13. Red No. 202 0.6 14. Yellow No. 4 2.2 15. KTP-09W (Note 2) 5 16. KF-9909 treated (Note 3) mica 2.5 17. Red No. 201 0.4 18. Isotridecyl isononanoate 4.5 19. Polyglyceryl-2 triisostearate 3.0 Total 100.0 (Note 1) Shin-Etsu Chemical Co., Ltd.: Diphenylsiloxyphenyl trimethicone (Note 2) Shin-Etsu Chemical Co., Ltd.: KF-9909 treated colored inorganic pigment, W: white, R: red, B: black (Note 3) Shin-Etsu Chemical Co., Ltd.: Triethoxysilylethyl polydimethylsiloxyethylhexyl dimethicone
[0171] (Production method) A: Components 13 to 19 were dispersed using a roll mill. B: Components 1 to 12 were mixed uniformly at 90°C. C: To the mixture obtained in B, the mixture obtained in A and component 19 were added, mixed uniformly at 80°C, filled into a mold, and slowly cooled to obtain a lipstick. The obtained lipstick had excellent adhesion, transfer resistance, and glossy feel, and also had a good feel in use.
[0172] Example 30 W / O Sunscreen Cream Composition % 1. KSG-820 (Note 1) 3.5 2. KSG-42A (Note 2) 3 3. KF-6105 (Note 3) 3 4. KF-4422 (Note 4) balance 5. Disteardimonium hectorite 1 6. Diethylamino hydroxybenzoyl hexyl benzoate 3 7. Bis-ethylhexyloxyphenol methoxyphenyl triazine 2 8. Ethylhexyl triazone 4 9. KF-56A (Note 5) 5 10. Dispersion of Example 14 15 11. Dispersion of Example 16 15 12. KSP-300 (Note 6) 1.5 13. BG 3 14. Ethanol 5 15. 15. Ethylhexylglycerin (as needed) 16. Sodium citrate (as needed) 17. Sodium chloride (as needed) 18. Purified water 30 Total 100.0 (Note 1) Shin-Etsu Chemical Co., Ltd.: Isododecane 70-80% + (Dimethicone / Polyglyceryl-3) Crosspolymer 20-30% mixture (Note 2) Shin-Etsu Chemical Co., Ltd.: Isododecane 75-85% + (Vinyl dimethicone / Lauryl dimethicone) Crosspolymer 15-25% mixture (Note 3) Shin-Etsu Chemical Co., Ltd.: Lauryl polyglyceryl-3 polydimethylsiloxyethyl dimethicone (Note 4) Shin-Etsu Chemical Co., Ltd.: Ethyl methicone (Note 5) Shin-Etsu Chemical Co., Ltd.: Diphenylsiloxyphenyl trimethicone(Note 6) Shin-Etsu Chemical Co., Ltd.: (Diphenyl dimethicone / vinyl diphenyl dimethicone / silsesquioxane) crosspolymer
[0173] (Production Method) A: Components 1 to 9 were mixed uniformly. B: Components 13 to 18 were mixed uniformly. C: The mixture obtained in B was added to the mixture obtained in A and emulsified, and components 10 to 12 were added to obtain a W / O sunscreen. The obtained W / O sunscreen contained a high blend of fine particle powder, but had low viscosity, high transparency, was non-sticky, and had a good feel when used. In addition, viscosity increase at high temperatures was suppressed, and it had excellent stability.
[0174] Examples 31 to 37 Oily paste dispersions were prepared according to the formulations shown in Table 6. (Production Method) Component (1) was dispersed using a roll to obtain an oily paste dispersion. (Note 1) Shin-Etsu Chemical Co., Ltd.: Caprylyl methicone (Note 2) Shin-Etsu Chemical Co., Ltd.: Diphenylsiloxyphenyl trimethicone (Note 3) Shin-Etsu Chemical Co., Ltd.: KF-9909 treated colored inorganic pigment, W: white, R: red, Y: yellow, B: black
[0175] Examples 38 to 44 Oily paste dispersions were prepared according to the formulations shown in Table 7. (Production Method) Component (1) was dispersed using a roll to obtain an oily paste dispersion. (Note 1) Shin-Etsu Chemical Co., Ltd.: Caprylyl methicone (Note 2) Shin-Etsu Chemical Co., Ltd.: Diphenylsiloxyphenyl trimethicone (Note 3) Shin-Etsu Chemical Co., Ltd.: KF-9909 treated colored inorganic pigment, W: white, R: red, Y: yellow, B: black, KF-9909 treated talc
[0176] Example 45 W / O Liquid Foundation Composition % 1. KSG-710 (Note 1) 4 2. KSG-43 (Note 2) 5 3. KF-6105 (Note 3) 4 4. TMF-1.5 (Note 4) balance 5. Organically modified clay mineral 1 6. Isononyl isononanoate 1 7. Cetyl ethylhexanoate 1.2 8. KF-7312L (Note 5) 2 9. KSP-300 (Note 6) 2 10. KF-56A (Note 7) 3 11. KF-4418 (Note 8) 3 12. Dispersion of any of Examples 31 to 44 20 13. BG 5 14. PCA-Na aqueous solution 1 15. Ethylhexylglycerin (as needed) 16. Pentylene glycol 1 17. Caprylyl glycol (as needed) 18. Sodium citrate (as needed) 19. Sodium chloride 0.520 Purified water 41.4 Total 100.0 (Note 1) Shin-Etsu Chemical Co., Ltd.: Dimethicone (6cs) 70-80% + (Dimethicone / Polyglycerin-3) Crosspolymer 20-30% Mixture (Note 2) Shin-Etsu Chemical Co., Ltd.: Triethylhexanoin 65-75% + (Vinyl Dimethicone / Lauryl Dimethicone) Crosspolymer 25-35% Mixture (Note 3) Shin-Etsu Chemical Co., Ltd.: Lauryl Polyglyceryl-3 Polydimethylsiloxyethyl Dimethicone (Note 4) Shin-Etsu Chemical Co., Ltd.: Methyl Trimethicone (Note 5) Shin-Etsu Chemical Co., Ltd.: Trimethylsiloxysilicate 50% Solution(Note 6) Shin-Etsu Chemical Co., Ltd.: (Diphenyl dimethicone / vinyl diphenyl dimethicone / silsesquioxane) crosspolymer (Note 7) Shin-Etsu Chemical Co., Ltd.: Diphenylsiloxyphenyl trimethicone (Note 8) Shin-Etsu Chemical Co., Ltd.: Caprylyl methicone
[0177] (Production method) A: Components 1 to 11 were mixed uniformly. B: Components 13 to 20 were mixed uniformly. C: The mixture obtained in B was added to the mixture obtained in A and emulsified, and component 12 was added to obtain a W / O liquid foundation. Although the obtained W / O liquid foundation contained a high powder content, it spread well and felt good in use.
[0178] [Example 46] W / O Cream Foundation Composition % 1. KSG-330 (Note 1) 3 2. KSG-18A (Note 2) 5 3. KF-6038 (Note 3) 1 4. KF-6048 (Note 4) 2 5. Organically modified clay mineral 1 6. Hexyl laurate 5 7. Homosalate 3 8. Bis-ethylhexyloxyphenol methoxyphenyl triazine 2 9. Ethylhexyl salicylate 3 10. KF-56A (Note 5) 3 11. KP-549 (Note 6) 3 12. Dispersion of any of Examples 31 to 44 15 13. BG 5 14. Betaine 1 15. Dipotassium glycyrrhizinate 0.1 16. Methyl glyceth-10 1 17. 17. Caprylhydroxamic acid Appropriate amount 18. Sodium citrate Appropriate amount 19. Sodium chloride 0.520. Purified water Remaining amount Total 100.0 (Note 1) Shin-Etsu Chemical Co., Ltd.: Mixture of triethylhexanoin 75-85% + (PEG-15 / lauryl dimethicone) crosspolymer 15-25% (Note 2) Shin-Etsu Chemical Co., Ltd.: Mixture of diphenylsiloxyphenyl trimethicone 80-90% + (dimethicone / phenyl vinyl dimethicone) crosspolymer 10-20% (Note 3) Shin-Etsu Chemical Co., Ltd.: Lauryl PEG-9 polydimethylsiloxyethyl dimethicone(Note 4) Shin-Etsu Chemical Co., Ltd.: Cetyl PEG / PPG-10 / 1 Dimethicone (Note 5) Shin-Etsu Chemical Co., Ltd.: Diphenylsiloxyphenyl Trimethicone (Note 6) Shin-Etsu Chemical Co., Ltd.: (Acrylates / Dimethicone) Copolymer 40% Solution
[0179] (Production method) A: Components 1 to 12 were mixed uniformly. B: Components 13 to 20 were mixed uniformly. C: The mixture obtained in A was added to the mixture obtained in B and emulsified to obtain a W / O cream foundation. The obtained W / O cream foundation contained a high powder content, but had good spreadability and a pleasant feel when used.
Claims
1. An organopolysiloxane represented by the following formula (1): [In the formula, R 1 are independently selected from an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, and an aralkyl group having 7 to 20 carbon atoms. 2 are each independently a divalent organic group having 3 to 15 carbon atoms which may be connected via an oxygen atom, p is 0≦p≦9, q is 0≦q≦200, r is 0≦r≦200, m is 0≦m≦10, n1 is 0≦n1≦5 (provided that when m=0 or 1, 1≦n1≦5), and n2 is an integer of 0≦n2≦5. However, the bonds of the glycerin units bracketed by m and n1 may be in blocks or random.] 2. The organopolysiloxane according to claim 1, wherein in said formula (1), n1=0 and m satisfies 0<m≦10.
3. The organopolysiloxane according to claim 2, wherein in said formula (1), p≠q.
4. The organopolysiloxane according to claim 1, wherein said organopolysiloxane has a weight average molecular weight in terms of polystyrene of 1,000 to 20,000.
5. The organopolysiloxane according to claim 1, wherein in said formula (1), q satisfies 0≦q≦9, and r satisfies 0≦r≦9.
6. The organopolysiloxane according to claim 1, wherein in said formula (1), q satisfies 10≦q≦200.
7. A cosmetic preparation comprising the organopolysiloxane according to any one of claims 1 to 6.
8. A dispersion comprising the organopolysiloxane according to any one of claims 1 to 6, a powder, and an oil.
9. The dispersion according to claim 8, wherein said organopolysiloxane is represented by formula (1), where q is 0≦q≦9 and r is 0≦r≦9, and the powder has an average primary particle size of less than 15 nm.
10. The dispersion according to claim 8, wherein in said organopolysiloxane, in said formula (1), q satisfies 10≦q≦200, and said powder has an average primary particle size of 15 nm or more.
11. A cosmetic preparation comprising the dispersion according to claim 8.
Citation Information
Patent Citations
Cosmetic
JP2002003334A
Powder dispersion stabilizer and powder dispersion composition with the powder dispersion stabilizer incorporated therein
JP2006218472A
Novel silicone powder treatment agent, powder surface-treated with the same, and cosmetics containing this powder
JP3912961B2
Cosmetic composition
WO2016178380A1
Organosilicon derivative and external preparation for skin
JP1994228167A