Dielectric ceramic composition and laminated ceramic electronic component

The dielectric ceramic composition with optimized elemental ratios and crystal grain locations addresses the insulation resistance challenge in multilayer ceramic capacitors, enhancing their performance in high-frequency and critical applications.

WO2024203277A1PCT designated stage expired Publication Date: 2024-10-03TAIYO YUDEN KK

Patent Information

Application Number
PCT/JP2024/009537
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-12
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Multilayer ceramic capacitors face a challenge in achieving high insulation resistance due to reduced grain boundaries and increased grain size, which affects their performance in high-frequency communication systems and critical applications like in-vehicle electronic control devices.

Method used

A dielectric ceramic composition with a perovskite structure containing barium titanate, magnesium, and manganese, along with nickel, is developed, where specific elemental ratios of these components are optimized to form first and second crystal grains that locate at grain boundaries, enhancing insulation resistance and reliability.

Benefits of technology

The optimized dielectric ceramic composition achieves high insulation resistance and reliability by precisely controlling the elemental ratios and locations of crystal grains, thereby improving the performance of multilayer ceramic capacitors in various electronic applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009537_03102024_PF_FP_ABST
    Figure JP2024009537_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The dielectric ceramic composition comprises: a main phase containing barium titanate having a perovskite structure; first crystal particles that satisfy 5.00≤a≤7.00 and 0.50≤b≤1.50 when the elemental ratio of titanium to the content of barium is taken as a and the elemental ratio of magnesium to the content of barium is taken as b; and second crystal particles that satisfy 1.50≤c≤3.50, 0.03≤d≤0.30, 0.03≤e≤0.30, and 0.03≤f≤0.40 when the elemental ratio of titanium to the content of barium is taken as c, the elemental ratio of magnesium to the content of barium is taken as d, the elemental ratio of manganese to the content of barium is taken as e, and the elemental ratio of nickel to the content of barium is taken as f. 
Need to check novelty before this filing date? Find Prior Art

Description

Dielectric ceramic composition and multilayer ceramic electronic component

[0001] The present invention relates to a dielectric ceramic composition and a multilayer ceramic electronic component.

[0002] 2. Description of the Related Art Multilayer ceramic electronic components such as multilayer ceramic capacitors (MLCCs) are used in high-frequency communication systems, such as mobile phones.

[0003] JP 2012-131669 A JP 2016-153359 A

[0004] The dielectric ceramic composition used in the dielectric layers of multilayer ceramic electronic components uses a sintered body with a core-shell structure, in which barium titanate is used as the core and is surrounded by a shell containing various additives in solid solution. This structure allows the large capacitance that occurs near the Curie temperature, around 125°C, where barium titanate changes from a ferroelectric phase to a paraelectric phase, to be transitioned to a lower temperature in the shell due to the effects of various additives, making it possible to design a device that can further increase capacitance in the practical temperature range around room temperature.

[0005] As an application example of barium titanate without a core-shell structure, Ba is used as a barium titanate composite oxide. 4 Ti 12 O 27 Or Ba 6 Ti 17 O 40 and further containing 0.04% by mass or more and 0.20% by mass or less of manganese in terms of metal relative to barium titanate (see, for example, Patent Document 1).

[0006] Also, (Ba 1-x Ca x ) a (Ti 1-y Zr y ) O 3(wherein 0.09≦x≦0.30, 0.025≦y≦0.085, 0.986≦a≦1.020) and 0.04 parts by weight or more and 0.36 parts by weight or less of manganese converted into metal relative to 100 parts by weight of the metal oxide, and the barium titanate composite oxide is BaTi 2 O 5 ,BaTi 4 O 9 ,BaTi 5 O 11 ,BaTi 6 O 13 ,BaTi 7 O 14 ,BaTi 8 O 16 , Ba 2 Ti 5 O 12 , Ba 2 Ti 6 O 13 , Ba 2 Ti 9 O 20 , Ba 4 Ti 11 O 26 , Ba 4 Ti 13 O 30 , CaTi 2 O 4 , CaTi 2 O 5 , CaTi 4 O 9 , Ca 2 Ti 5 O 12 , CaZr 4 O 9 , Ca 2 Zr 7 O 16 , Ca 6 Zr 19 O 44 , CaZrTi 2 O 7 , and Ca 2 Zr 5 Ti 2 O 16 , and JP-A-2003-129999 discloses a piezoelectric ceramic containing at least one metal oxide selected from the group consisting of:

[0007] When attempts were made to apply the piezoelectric ceramics disclosed in Patent Documents 1 and 2 to a dielectric ceramic composition used in the dielectric layers of multilayer ceramic electronic components, it was confirmed that the maximum grain size of the crystal grains was 2 μm or more, as disclosed in Patent Documents 1 and 2. In multilayer ceramic electronic components in which the dielectric layers were 10 μm or less, the number of grain boundaries was reduced, resulting in a problem of significant deterioration in insulation resistance.

[0008] In recent years, the use of multilayer ceramic capacitors has expanded to include electronic circuits that affect human life, such as in-vehicle electronic control devices, making it necessary to ensure high insulation resistance.

[0009] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a dielectric ceramic composition and a multilayer ceramic electronic component that can achieve high insulation resistance.

[0010] The dielectric ceramic composition according to the present invention has a main phase containing barium titanate having a perovskite structure; first crystal particles containing barium, titanium, and magnesium, wherein, where a is the atomic ratio of titanium to the barium content and b is the atomic ratio of magnesium to the barium content, the ratios are 5.00≦a≦7.00 and 0.50≦b≦1.50; and second crystal particles containing barium, titanium, magnesium, manganese, and nickel, the ratios are 1.50≦c≦3.50, 0.03≦d≦0.30, 0.03≦e≦0.30, and 0.03≦f≦0.40, where c is the atomic ratio of titanium to the barium content, d is the atomic ratio of magnesium to the barium content, e is the atomic ratio of manganese to the barium content, and f is the atomic ratio of nickel to the barium content.

[0011] In the above dielectric ceramic composition, the first crystal particles may further contain manganese and nickel, and when the elemental ratio of manganese to the content of barium in the first crystal particles is g and the elemental ratio of nickel to the content of barium in the first crystal particles is h, 0.10≦g≦4.00 and 0.10≦h≦4.00 may be satisfied.

[0012] The dielectric ceramic composition may further include third crystal particles containing at least one of silicate, enstatite, barium magnesium silicate, and fresnoite.

[0013] In the above dielectric ceramic composition, the first crystal grains and the second crystal grains may be located at grain boundaries of the main phase.

[0014] In the above dielectric ceramic composition, the first crystal grains and the second crystal grains may be located at grain boundary triple junctions of the main phase.

[0015] In the above dielectric ceramic composition, the third crystal grains may be located at the grain boundaries of the main phase.

[0016] In the above dielectric ceramic composition, the third crystal grains may be located at the grain boundary triple junction of the main phase.

[0017] In the above dielectric ceramic composition, the main phase may have a core portion and a shell portion covering the core portion.

[0018] In the dielectric ceramic composition, the shell portion may contain a rare earth element.

[0019] In the dielectric ceramic composition, the element ratio of barium to titanium may be 0.940 or more and 0.980 or less, the element ratio of gadolinium to titanium may be 0.005 or more and 0.05 or less, and the element ratio of magnesium to titanium may be 0.002 or more and 0.02 or less.

[0020] Another dielectric ceramic composition according to the present invention has a perovskite structure, a main phase containing barium titanate, and having a core portion and a shell portion covering the core portion, and first crystal particles containing barium, titanium, and magnesium, wherein, when the elemental ratio of titanium to the barium content is a and the elemental ratio of magnesium to the barium content is b, the relationship is 5.00≦a≦7.00 and 0.50≦b≦1.50.

[0021] In the above dielectric ceramic composition, the first crystal particles may further contain manganese and nickel, and when the elemental ratio of manganese to the content of barium in the first crystal particles is g and the elemental ratio of nickel to the content of barium in the first crystal particles is h, 0.10≦g≦4.00 and 0.10≦h≦4.00 may be satisfied.

[0022] A multilayer ceramic electronic component according to the present invention comprises a plurality of dielectric layers containing a dielectric ceramic composition, a plurality of internal electrodes facing each other with the plurality of dielectric layers interposed therebetween, and external electrodes electrically connected to the plurality of internal electrodes.

[0023] According to the present invention, it is possible to provide a dielectric ceramic composition and a multilayer ceramic electronic component that can achieve high insulation resistance.

[0024] 3 is a diagram illustrating a dielectric ceramic composition according to a first embodiment; FIG. 4 is a diagram illustrating a unit cell; FIG. 5 is a partial cross-sectional perspective view of a multilayer ceramic capacitor; FIG. 6 is a cross-sectional view taken along line A-A in FIG. 3; FIG. 7 is a cross-sectional view taken along line B-B in FIG. 3; FIG. 8 is a diagram illustrating a flow of a method for manufacturing a multilayer ceramic capacitor; (a) and (b) are diagrams illustrating an internal electrode forming step; (b) are diagrams illustrating a pressure bonding step; and (c) are diagrams illustrating a side margin portion.

[0025] Hereinafter, embodiments will be described with reference to the drawings.

[0026] (First embodiment) The dielectric ceramic composition according to the first embodiment is represented by the general formula ABO 3 These ceramic polycrystalline bodies include crystal grains having a perovskite structure represented by the formula: As shown in FIG. 1 , these ceramic polycrystalline bodies include main phase crystal grains 40 and first crystal grains 41.

[0027] The main phase crystal grains 40 contain barium titanate having a perovskite structure. The first crystal grains 41 contain barium, titanium, and magnesium, and when the elemental ratio of titanium to the barium content is a (hereinafter also referred to as Ti / Ba elemental ratio a) and the elemental ratio of magnesium to the barium content is b (hereinafter also referred to as Mg / Ti elemental ratio b), the relationship is 5.00≦a≦7.00 and 0.50≦b≦1.50.

[0028] For example, when a cross section of the dielectric ceramic composition is observed in a field of view where a total of 400 or more main phase crystal grains 40 and first crystal grains 41 can be confirmed, the area ratio of the main phase crystal grains 40 is 50.0% or more and 99.95% or less, and the area ratio of the first crystal grains 41 is 0.050% or more and 45.0% or less.

[0029] The barium titanate crystal grains having a perovskite structure, which are the main component of the main phase crystal grains 40, have a unit lattice as shown in Fig. 2. This unit lattice has A sites located at the vertices of the lattice, O sites located at the face centers of the lattice, and B sites located within octahedra with the O sites as vertices. In the perovskite structure, alkaline earth metals that can take divalent cations, such as barium (Ba), strontium (Sr), and calcium (Ca), are located at the A sites, and metal atoms that can take tetravalent cations, such as hafnium (Hf), zirconium (Zr), and titanium (Ti), are located at the B sites.

[0030] The perovskite structure also allows for a composition formula that deviates from the stoichiometric composition. That is, the ratio of the A-site element to the B-site element does not necessarily have to be 1:1, and defects may be generated within a range that allows the perovskite structure to be maintained. Also, defects may be generated in oxygen. For example, in the composition formula A α BO 3-β When this is the case, a composition in the ranges of 0.98≦α≦1.01 and 0≦β≦0.20 is acceptable.

[0031] However, for example, the generation of oxygen defects can reduce resistivity and exhibit ionic conductivity, which can shorten the electrical life and increase dielectric loss when used as a multilayer ceramic capacitor, making it unsuitable for practical use. For this reason, the main phase crystal grains 40 having a perovskite structure may contain at least one alkaline earth element selected from magnesium (Mg), calcium (Ca), strontium (Sr), and barium (Ba), as needed. This can improve resistivity, increase electrical life, and reduce dielectric loss relative to capacitance.

[0032] Furthermore, the main phase crystal grains 40 may contain at least one of the first transition elements scandium (Sc), titanium (Ti), vanadium (V), chromium (Cr), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), and zinc (Zn), as needed, which can improve resistivity, increase electrical life, and reduce dielectric loss relative to capacitance.

[0033] Furthermore, the main phase crystal grains 40 may contain at least one of the second transition elements yttrium (Y), zirconium (Zr), niobium (Nb), molybdenum (Mo), ruthenium (Ru), rhodium (Rh), palladium (Pd), and silver (Ag) as needed, which can improve resistivity, increase electrical life, and reduce dielectric loss relative to capacitance.

[0034] Furthermore, the main phase crystal grains 40 may contain at least one of the third transition elements lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), hafnium (Hf), tantalum (Ta), tungsten (W), rhenium (Re), osmium (Os), iridium (Ir), platinum (Pt), and gold (Au), as needed, which can improve resistivity, increase electrical life, and reduce dielectric loss relative to capacitance.

[0035] By using at least one of the alkaline earth element, first transition metal element, second transition metal element, and third transition metal element as an additive, at least one of the alkaline earth element, first transition metal element, second transition metal element, and third transition metal element can be solid-dissolved from the interface of the main phase crystal grain 40 to the inside in the firing temperature range of 1000°C to 1400°C for obtaining the dielectric ceramic composition, thereby forming the core portion 411 and the shell portion 412 in the main phase crystal grain 40. For example, the dielectric ceramic composition can be prepared by mixing 100 mol of gadolinium oxide (Gd) with 100 mol of barium titanate so that the Gd / Ti element ratio j, which is the element ratio of gadolinium to the content of barium, satisfies 0.005≦j≦0.05. 2 O 3 It is preferable to add 0.25 mol or more and 2.5 mol or less of gadolinium in terms of MgO. In addition to the addition of gadolinium oxide, it is preferable to add 0.2 mol or more and 2.0 mol or less of magnesium oxide (MgO) in terms of MgO to 100 mol of barium titanate so that the Mg / Ti element ratio k, which is the magnesium element ratio to the barium content, satisfies 0.002≦k≦0.05. For example, when 0.005≦j≦0.05 and 0.002≦k≦0.02 are satisfied, the added gadolinium, manganese, and titanium react on the surface of the barium titanate crystal particles to form Gd(Ti,Mg)O. 3The shell portion can be formed in the form of a composite perovskite compound that is thought to be a composite perovskite compound. This makes it possible for the dielectric ceramic composition to suppress the migration of oxygen defects at the grain boundaries and inside the shell portion, suppress the decrease in resistivity, and improve the electrical life.

[0036] In a core-shell structure, generally, as the firing temperature increases, various additives tend to dissolve in greater amounts in the crystal particles of barium titanate, resulting in a thicker shell portion 412 and a smaller particle size in the core portion 411. In the shell portion 412, an acceptor element with a lower valence than titanium, such as magnesium, dissolves as a B-site element, thereby suppressing the reduction of titanium during reduction firing and improving insulation resistance. Therefore, for example, to ensure high insulation resistance in a multilayer ceramic capacitor, it is necessary to dissolve the acceptor element in the shell portion 412.

[0037] However, when the acceptor element dissolves in the shell portion 412, oxygen defects are generated, which may reduce the electrical life and reliability. Therefore, in order to achieve both high insulation resistance and high reliability, it is necessary to precisely control the amount of the acceptor element dissolved in the shell portion 412.

[0038] The dielectric ceramic composition according to this embodiment includes, in addition to main phase crystal grains 40 containing barium titanate having a perovskite structure, first crystal grains 41 satisfying the following conditions: 5.00≦Ti / Ba element ratio a≦7.00, and 0.50≦Mg / Ba element ratio b≦1.50. By intentionally precipitating the first crystal grains 41 in this manner, high reliability and high insulation resistance can be achieved. The Ti / Ba element ratio a is preferably 5.15 or more, and more preferably 5.40 or more, which allows high insulation resistance to be achieved. Furthermore, the Ti / Ba element ratio a is preferably 6.85 or less, and more preferably 6.60 or less, which allows high insulation resistance to be achieved. The Mg / Ba element ratio b is preferably 0.60 or more, and more preferably 0.75 or more, which allows high insulation resistance to be achieved. The Mg / Ba element ratio b is preferably 1.40 or less, and more preferably 1.25 or less, since a high insulation resistance can be achieved.

[0039] The first crystal particles 41 further contain manganese and nickel, and when the elemental ratio of manganese to the barium content is g (hereinafter also referred to as the Mn / Ba elemental ratio g) and the elemental ratio of nickel to the barium content is h (hereinafter also referred to as the Ni / Ba elemental ratio h), it is preferable that 0.10≦g≦4.00 and 0.10≦h≦4.00 are satisfied. This is because a decrease in the resistivity of the dielectric ceramic composition can be suppressed. The Mn / Ba elemental ratio g is more preferably 0.50 or more, and even more preferably 1.00 or more, which can achieve high insulation resistance. The Mn / Ba elemental ratio g is more preferably 3.75 or less, and even more preferably 3.50 or less, which can achieve high insulation resistance. The Ni / Ba elemental ratio h is preferably 0.50 or more, and even more preferably 1.00 or more, which can achieve high insulation resistance. The Ni / Ba element ratio h is preferably 3.75 or less, and more preferably 3.50 or less, since a high insulation resistance can be achieved.

[0040] The first crystal particles 41 may also contain at least one of calcium, scandium, vanadium, chromium, iron, cobalt, nickel, copper, zinc, yttrium, zirconium, niobium, and molybdenum, because this can suppress a decrease in the resistivity of the dielectric ceramic composition.

[0041] The presence of the first crystal particles 41 in the dielectric ceramic composition can be confirmed by the following procedure.

[0042] First, the surface of the dielectric ceramic composition is exposed. This exposure method is not particularly limited, and methods such as cutting or polishing the element can be used. In this case, to fully observe the internal ceramic structure, it is preferable to finally obtain a smoothness that can be considered a mirror surface using a diamond paste or the like of 2 microns or less. The above-mentioned method of cutting or polishing the element is suitable for observation by SEM. Furthermore, a thin section with a thickness of 100 nm or less can also be obtained from the surface of the dielectric ceramic composition that has a smoothness that can be considered a mirror surface using an ion beam or the like. The thin section is suitable for observation by STEM.

[0043] Next, the composition of the first crystal particles 41 is identified using an energy dispersive X-ray spectrometry (EDS) or wavelength dispersive X-ray spectrometry (WDS) attached to a scanning electron microscope (SEM) or a scanning transmission electron microscope (STEM), an electron probe microanalyzer (EPMA), a laser irradiation inductively coupled plasma mass spectrometry (LA-ICPMS), or the like.

[0044] For example, in EDS measurement, they are simply identified by the K-line intensity of titanium and the K-line intensity of magnesium relative to the K-line or L-line of barium. More specifically, correction (ZAF correction) is performed from these intensities, taking into account the atomic number effect, absorption effect, and fluorescence excitation effect, to calculate the ratio of each element to the barium element content, which is then used as the ratio of each element.

[0045] When EDS measurement is performed, particularly in the measurement using barium Lα rays and titanium Kα rays, the energy peaks are close to each other, making it difficult to sufficiently compare the element contents.For this reason, it is desirable that the barium Lβ2 rays and LIIIab rays are obtained with sufficient intensity without peak overlap during measurement.Specifically, it is desirable that the intensity at the peak is 10,000 counts or more.At this time, the intensity of the characteristic X-rays of barium can be identified and the element content can be calculated.Therefore, even if the barium Lα rays and titanium Kα rays overlap, the intensity of the titanium Kα rays can be identified and the element content can be evaluated with high accuracy.

[0046] When crystal particles obtained by the above method are confirmed to have a Ti / Ba element ratio a of 5.00 or more and 7.00 or less and a Mg / Ba element ratio b of 0.50 or more and 1.50 or less, the crystal particles can be determined to be first crystal particles 41. That is, the first crystal particles 41 are determined to be barium titanate composite oxide because the element ratio of titanium and magnesium to barium is higher than that of the surrounding main phase crystal particles 40 made of barium titanate. When an SEM is used for observation, the first crystal particles 41 are characterized by being observed to have a relatively low brightness and appear darker than the main phase crystal particles 40 in a backscattered electron image (BSE image). Furthermore, when STEM is used for observation, in observation using a high-angle annular dark-field scanning transmission electron microscopy image (HAADF-STEM image), the first crystal grains 41 are characterized in that they have a relatively low brightness and are observed to appear dark compared to the main phase crystal grains 40.

[0047] Furthermore, when quantifying the manganese content and nickel content of the first crystal particles 41, they are simply quantified using the K-line intensity of manganese and the K-line intensity of nickel relative to the K-line or L-line of barium. More specifically, from these intensities, a correction (ZAF correction) taking into account the atomic number effect, absorption effect, and fluorescence excitation effect is performed to calculate the ratio of each element to the element content of barium, which is used as the ratio of each element. Furthermore, if the particle diameter of the first crystal particles 41 is smaller than the spatial resolution of EDS analysis using an SEM, it is desirable to observe the first crystal particles 41 using a scanning transmission electron microscope (STEM) and identify the composition of the first crystal particles 41 using EDS.

[0048] As illustrated in FIG. 1 , the dielectric ceramic composition preferably includes second crystal particles 42 in addition to main phase crystal particles 40 and first crystal particles 41. The second crystal particles 42 contain barium, titanium, magnesium, manganese, and nickel, and satisfy the following relationships: 1.50≦Ti / Ba elemental ratio c≦3.50, 0.03≦Mg / Ba elemental ratio d≦0.30, 0.03≦Mn / Ba elemental ratio e≦0.30, and 0.03≦Ni / Ba elemental ratio f≦0.40, where c is the elemental ratio of titanium to the barium content (hereinafter also referred to as Ti / Ba elemental ratio c), d is the elemental ratio of magnesium to the barium content (hereinafter also referred to as Mg / Ba elemental ratio d), e is the elemental ratio of manganese to the barium content (hereinafter also referred to as Mn / Ba elemental ratio e), and f is the elemental ratio of nickel to the barium content (hereinafter also referred to as Ni / Ba elemental ratio f).

[0049] For example, when a cross section of the dielectric ceramic composition is observed in a field of view where a total of 400 or more main phase crystal grains 40, first crystal grains 41, and second crystal grains 42 can be confirmed, the area ratio of the main phase crystal grains 40 is 50.0% or more and 99.95% or less, the area ratio of the first crystal grains 41 is 0.050% or more and 45.0% or less, and the area ratio of the second crystal grains 42 is 0.050% or more and 15.0% or less.

[0050] The second crystal particles 42 are crystal particles that are generated secondarily when an additive containing titanium as a main component is used. By intentionally precipitating the second crystal particles 42, the main phase crystal particles 4 and the first crystal particles 41 are obtained, and high insulation resistance can be obtained in a multilayer ceramic capacitor that requires high reliability.

[0051] The Ti / Ba element ratio c is more preferably 1.70 or more, and even more preferably 1.90 or more to achieve high insulation resistance. The Ti / Ba element ratio c is more preferably 2.70 or less, and even more preferably 2.50 or less to achieve high insulation resistance. The Mg / Ba element ratio d is preferably 0.05 or more, and even more preferably 0.08 or more to achieve high insulation resistance. The Mg / Ba element ratio d is preferably 0.25 or less, and even more preferably 0.20 or less to achieve high insulation resistance. The Mn / Ba element ratio e is more preferably 0.05 or more, and even more preferably 0.08 or more to achieve high insulation resistance. The Mn / Ba element ratio e is more preferably 0.25 or less, and even more preferably 0.20 or less to achieve high insulation resistance. The Ni / Ba element ratio f is preferably 0.05 or more, and more preferably 0.10 or more to achieve high insulation resistance, and is preferably 0.35 or less, and more preferably 0.30 or less to achieve high insulation resistance.

[0052] The second crystal particles 42 may further contain at least one of calcium, scandium, vanadium, chromium, iron, cobalt, nickel, copper, zinc, yttrium, zirconium, niobium, and molybdenum, because this can suppress a decrease in the resistivity of the dielectric ceramic composition.

[0053] Whether the dielectric ceramic composition contains the second crystal particles 42 can be confirmed by the following procedure.

[0054] First, the surface of the dielectric ceramic composition is exposed. This exposure method is not particularly limited, and methods such as cutting or polishing the element can be used. At this time, in order to fully observe the internal ceramic structure, it is preferable to finally obtain a smoothness that can be judged as a mirror surface using a diamond paste or the like of 2 microns or less. The above-mentioned method of cutting or polishing the element is suitable for observation by SEM. Furthermore, a thin section with a thickness of 100 nm or less can also be obtained from the surface of the dielectric ceramic composition that has a smoothness that can be judged as a mirror surface using an ion beam or the like. The thin section is suitable for observation by STEM.

[0055] Next, the composition of the second crystal particles 42 is identified by EDS or WDS, EPMA, LA-ICPMS, or the like attached to the SEM or STEM.

[0056] For example, in EDS measurements, the elements are simply identified by the K-line intensity of titanium, magnesium, manganese, and nickel relative to the K-line or L-line of barium. More specifically, corrections (ZAF corrections) that take into account atomic number effects, absorption effects, and fluorescence excitation effects are performed from these intensities, and the ratios of each element relative to the barium element content are calculated, which is used as the ratio of each element. When the sample thickness is sufficiently thin, for example, less than several tens of nanometers, corrections can be performed using the proportionality coefficient (K factor) used in the Cliff-Florimer method to determine the ratio of each element. Furthermore, in addition to the corrections used in the Cliff-Florimer method, corrections that take into account the absorption effect of the sample can be performed to determine the ratio of each element. The absorption effect of the sample can be corrected by determining the thickness and density of the sample. The thickness of the sample can be determined, for example, by obtaining a convergent-beam electron diffraction (CBED) pattern under two-wave excitation conditions and analyzing the rocking curve observed on a diffraction disk. The particles from which the CBED pattern is obtained can be the main phase crystal grains 40 or the like. The density of the sample can be, for example, 6.02 g / cm, which is the density of barium titanate. 3 Values ​​such as:

[0057] When EDS measurement is performed, particularly in the measurement using barium Lα rays and titanium Kα rays, the energy peaks are close to each other, making it difficult to sufficiently compare the element contents.For this reason, it is desirable that the barium Lβ2 rays and LIIIab rays are obtained with sufficient intensity without peak overlap during measurement.Specifically, it is desirable that the intensity at the peak is 10,000 counts or more.At this time, the intensity of the characteristic X-rays of barium can be identified and the element content can be calculated.Therefore, even if the barium Lα rays and titanium Kα rays overlap, the intensity of the titanium Kα rays can be identified and the element content can be evaluated with high accuracy.

[0058] When crystal particles are confirmed that have a Ti / Ba elemental ratio c of 1.50≦c≦3.50, a Mg / Ba elemental ratio d of 0.03≦d≦0.30, a Mn / Ba elemental ratio e of 0.03≦e≦0.30, and a Ni / Ba elemental ratio f of 0.03≦f≦0.40 obtained by the above method, the crystal particles can be determined to be second crystal particles 42. That is, second crystal particles 42 are determined to be barium titanate composite oxide because the elemental ratios of titanium, magnesium, manganese, and nickel to barium are higher than those of the surrounding main phase crystal particles 40 made of barium titanate and the elemental ratios of titanium, magnesium, manganese, and nickel to barium are lower than those of the first crystal particles 41. When an SEM is used for the observation, the second crystal particles 42 are characterized in that, in observation using a backscattered electron image (BSE image), the second crystal particles 42 are observed to have a relatively low brightness and appear darker than the main phase crystal particles 40. When an STEM is used for the observation, the second crystal particles 42 are characterized in that, in observation using a high-angle annular dark-field scanning transmission electron microscopy image (HAADF-STEM image), the second crystal particles 42 are characterized in that, in observation using a high-angle annular dark-field scanning transmission electron microscopy image (HAADF-STEM image), the second crystal particles 42 are observed to have a relatively low brightness and appear darker than the main phase crystal particles 40. Furthermore, when quantifying the manganese content and nickel content of the second crystal particles 42, they are simply quantified using the manganese K-line intensity and nickel K-line intensity relative to the barium K-line or L-line. More specifically, these intensities are subjected to a correction (ZAF correction) that takes into account the atomic number effect, absorption effect, and fluorescence excitation effect, and the ratio of each element relative to the barium element content is calculated, which is then used as the ratio of each element. If the sample thickness is sufficiently thin, for example, less than several tens of nanometers, a correction using the proportionality coefficient (K factor) used in the Cliff-Florimer method may be performed to determine the ratio of each element. Furthermore, in addition to the correction used in the Cliff-Florimer method, a correction that takes into account the absorption effect of the sample may be performed to determine the ratio of each element. The absorption effect of the sample can be corrected by determining the thickness and density of the sample.The thickness of the sample can be determined, for example, by obtaining a convergent-beam electron diffraction (CBED) pattern under two-wave excitation conditions and analyzing the rocking curve observed on a diffraction disk. The particles from which the CBED pattern is obtained can be the main phase crystal grains 40 or the like. The density of the sample is, for example, 6.02 g / cm, which is the density of barium titanate. 3 Values ​​such as:

[0059] Furthermore, when the particle diameter of the second crystal particles 42 is smaller than the spatial resolution of EDS analysis using an SEM, it is desirable to identify the composition of the second crystal particles 42 using a scanning transmission electron microscope (STEM).

[0060] The dielectric ceramic composition may contain, in addition to the main phase crystal grains 40, the first crystal grains 41, and the second crystal grains 42, third crystal grains 43 having a different composition or crystal structure from these, voids 44, etc. For example, when a cross section of the dielectric ceramic composition is observed in a field where a total of 400 or more main phase crystal grains 40, first crystal grains 41, second crystal grains 42, and third crystal grains 43 can be confirmed, the area ratio of the third crystal grains 43 is 0.050% or more and 15.0% or less.

[0061] The third crystal particles 43 are made of silicate (SiO 2 ), enstatite (MgSiO 3 ), barium magnesium silicate (BaMgSiO 4 ), Fresnoit (Ba 2 TiSi 2 O 8 The inclusion of the third crystal particles makes it possible to sinter the dielectric ceramic composition at 1300°C or less and to achieve sufficient densification. Instead of the third crystal particles 43, silicate (SiO 2 ), enstatite (MgSiO 3 ), barium magnesium silicate (BaMgSiO 4 ), Fresnoit (Ba 2 TiSi 2 O8 Glass particles such as SiO 2 may be included in the dielectric ceramic composition.

[0062] The dielectric ceramic composition includes main phase crystal grains 40, first crystal grains 41, second crystal grains 42, and third crystal grains 43, as well as geikierite (MgTiO 3 ), manganese nickel oxide ((Mn,Ni)O), pyrophanite (MnTiO 3 ) or secondary compounds derived from the electrode.

[0063] As illustrated in Fig. 1, the first crystal grains 41 and the second crystal grains 42 are preferably located at the grain boundaries of the main phase crystal grains 40. This is because a decrease in the resistivity of the dielectric ceramic composition can be suppressed.

[0064] The first crystal grains 41 and the second crystal grains 42 are preferably located at the grain boundary triple junctions of the main phase crystal grains 40. This is because a decrease in the resistivity of the dielectric ceramic composition can be suppressed. The grain boundary triple junctions are the boundaries between three crystal grain boundaries.

[0065] The third crystal grains 43 are preferably located at the grain boundaries of the main phase crystal grains 40. This is because a decrease in the relative dielectric constant of the dielectric ceramic composition can be suppressed.

[0066] The third crystal grains 43 are preferably located at the grain boundary triple points of the main phase crystal grains 40. This is because a decrease in the relative dielectric constant of the dielectric ceramic composition can be suppressed.

[0067] It is preferable that the shell portion 412 of the main phase crystal grain 40 contains a rare earth element, because this improves the life of the dielectric ceramic composition.

[0068] In the main phase crystal grains 40, the first crystal grains 41, the second crystal grains 42, and the third crystal grains 43 as a whole, the element ratio of titanium to the barium content is preferably greater than 0.940 and not more than 0.980, because a sufficient number of first crystal grains 41 and second crystal grains 42 are generated.

[0069] Second Embodiment In a second embodiment, a multilayer ceramic capacitor 100 using the dielectric ceramic composition according to the first embodiment will be described.

[0070] FIG. 3 is a partial cross-sectional perspective view of the multilayer ceramic capacitor 100. FIG. 4 is a cross-sectional view taken along line A-A in FIG. 3. FIG. 5 is a cross-sectional view taken along line B-B in FIG. 3. As illustrated in FIGS. 3 to 5, the multilayer ceramic capacitor 100 includes a laminated chip 10 having a substantially rectangular parallelepiped shape and external electrodes 20a, 20b provided on two opposing end faces of the laminated chip 10. Of the four faces of the laminated chip 10 other than the two end faces, the two faces other than the top and bottom faces in the stacking direction are referred to as side faces. The external electrodes 20a, 20b extend on the top, bottom, and two side faces of the laminated chip 10 in the stacking direction. However, the external electrodes 20a, 20b are spaced apart from each other.

[0071] The multilayer chip 10 has a configuration in which dielectric layers 11 containing a dielectric ceramic composition and internal electrode layers 12 containing a base metal material are alternately stacked. The edges of each internal electrode layer 12 are alternately exposed at the end face of the multilayer chip 10 on which the external electrode 20a is provided and the end face on which the external electrode 20b is provided. As a result, each internal electrode layer 12 is alternately electrically connected to the external electrode 20a and the external electrode 20b. As a result, the multilayer ceramic capacitor 100 has a configuration in which multiple dielectric layers 11 are stacked with the internal electrode layers 12 interposed therebetween. In addition, in a laminate of the dielectric layers 11 and the internal electrode layers 12, the internal electrode layer 12 is disposed as the outermost layer in the stacking direction, and the upper and lower surfaces of the laminate are covered by cover layers 13. The cover layers 13 are primarily composed of a ceramic material. For example, the material of the cover layers 13 may have the same primary ceramic material as that of the dielectric layers 11.

[0072] The size of the multilayer ceramic capacitor 100 is, for example, 0.25 mm in length, 0.125 mm in width, and 0.125 mm in height, or 0.4 mm in length, 0.2 mm in width, and 0.2 mm in height, or 0.6 mm in length, 0.3 mm in width, and 0.3 mm in height, or 1.0 mm in length, 0.5 mm in width, and 0.5 mm in height, or 3.2 mm in length, 1.6 mm in width, and 1.6 mm in height, or 4.5 mm in length, 3.2 mm in width, and 2.5 mm in height, but is not limited to these sizes.

[0073] The internal electrode layers 12 are mainly composed of base metals such as Ni (nickel), Cu (copper), Sn (tin), etc. The internal electrode layers 12 may also be made of precious metals such as Pt (platinum), Pd (palladium), Ag (silver), Au (gold), etc., or alloys containing these metals.

[0074] 4, the region where the internal electrode layer 12 connected to the external electrode 20a and the internal electrode layer 12 connected to the external electrode 20b face each other is a region where capacitance is generated in the multilayer ceramic capacitor 100. Therefore, this region where capacitance is generated is referred to as a capacitance region 14. In other words, the capacitance region 14 is a region where adjacent internal electrode layers 12 connected to different external electrodes face each other.

[0075] The region where the internal electrode layers 12 connected to the external electrode 20a face each other without an internal electrode layer 12 connected to the external electrode 20b interposed therebetween is called the end margin 15. The region where the internal electrode layers 12 connected to the external electrode 20b face each other without an internal electrode layer 12 connected to the external electrode 20a interposed therebetween is also the end margin 15. In other words, the end margin 15 is the region where the internal electrode layers 12 connected to the same external electrode face each other without an internal electrode layer 12 connected to a different external electrode interposed therebetween. The end margin 15 is a region where no electrical capacitance is generated.

[0076] 5, in the laminated chip 10, the regions extending from the two side surfaces of the laminated chip 10 to the internal electrode layers 12 are referred to as side margins 16. In other words, the side margins 16 are regions provided to cover the ends of the multiple internal electrode layers 12 stacked in the above-mentioned laminated structure that extend to the two side surfaces. The side margins 16 are also regions that do not generate electrical capacitance.

[0077] In the multilayer ceramic capacitor 100 according to this embodiment, the main phase crystal grains 40 and the first crystal grains 41 illustrated in Fig. 1 are contained in at least a portion of the dielectric layer 11 in the capacitance region 14. This makes it possible to achieve high reliability and high insulation resistance.

[0078] Next, a method for manufacturing the multilayer ceramic capacitor 100 will be described. Figure 6 is a diagram illustrating the flow of the method for manufacturing the multilayer ceramic capacitor 100.

[0079] (Step of Preparing Raw Material Powder) First, a dielectric ceramic composition for forming the dielectric layer 11 is prepared. The A-site elements and B-site elements contained in the dielectric layer 11 are usually ABO 3 The dielectric layer 11 is formed of a sintered body of particles of the above-mentioned material. For example, barium titanate is a compound that has a perovskite structure and belongs to the tetragonal system at around room temperature, and exhibits a high relative dielectric constant. This barium titanate can generally be synthesized by reacting a titanium raw material such as titanium dioxide with a barium raw material such as barium carbonate. Various methods have been known for synthesizing barium titanate, which is the main component of the dielectric layer 11, including the solid-phase method, the sol-gel method, and the hydrothermal method. Any of these methods can be used in this embodiment.

[0080] Predetermined additives are added to the barium titanate powder obtained by the above method. As an example, additives within the ranges shown in the example of the dielectric ceramic composition according to the first embodiment are used. If necessary, oxides or glasses containing Zr (zirconium), V (vanadium), Cr (chromium), Co (cobalt), Ni (nickel), Li (lithium), B (boron), Na (sodium), and K (potassium) may be used. Furthermore, if necessary, oxides of rare earth elements such as Sc (scandium), Y (yttrium), La (lanthanum), Ce (cerium), Pr (praseodymium), Nd (neodymium), Pm (promethium), Sm (samarium), Tb (terbium), Dy (dysprosium), Ho (holmium), Er (erbium), Tm (thulium), Y (ytterbium), and Lu (lutetium) may be added.

[0081] In order to generate the first crystal particles 41, titanium oxide (TiO 2It is preferable to add an additive whose main component is titanium in an amount of 0.002 mol or more and 0.06 mol or less in terms of magnesium oxide (MgO), and an additive whose main component is magnesium in an amount of 0.002 mol or more and 0.05 mol or less in terms of magnesium oxide (MgO). This produces the first crystal particles 41. Note that as an additive whose main component is titanium, titanium hydroxide (Ti(OH) 4 ), titanium chloride (TiCl 4 ), titanium carbide (TiC), titanium sulfide (TiS 2 ) may be used. In addition to magnesium oxide, magnesium hydroxide (MgOH), magnesium chloride (MgCl 2 ), magnesium carbonate (MgCO 3 ), magnesium sulfide (MgS), etc. may also be used.

[0082] In order to generate the second crystal particles 42, titanium oxide (TiO 2 an additive containing titanium as a main component in an amount of 0.002 mol or more and 0.08 mol or less in terms of magnesium oxide (MgO) is added, an additive containing magnesium as a main component in an amount of 0.002 mol or more and 0.05 mol or less in terms of manganese carbonate (MnCO 3 It is preferable to add an additive containing manganese as the main component in an amount of 0.002 mol or more and 0.05 mol or less in terms of manganese (calculated as 0.002 mol or more). This produces the second crystal particles 42. As an additive containing titanium as the main component, titanium hydroxide (Ti(OH) 4 ), titanium chloride (TiCl 4 ), titanium carbide (TiC), titanium sulfide (TiS 2 ) may be used. In addition to magnesium oxide, magnesium hydroxide (MgOH) and magnesium chloride (MgCl) may also be used as additives containing magnesium as the main component. 2 ), magnesium carbonate (MgCO 3 ), magnesium sulfide (MgS), etc. may also be used. In addition to manganese carbonate, manganese monoxide (MnO) and manganese trioxide (Mn 3 O 4), manganese dioxide (MnO 2 ) etc. may also be used.

[0083] For example, a compound containing an additive compound is wet mixed with barium titanate powder, followed by drying and pulverization to prepare a ceramic material containing the barium titanate powder and the additive compound. For example, the ceramic material obtained as described above may be pulverized as necessary to adjust the particle size, or may be combined with a classification process to adjust the particle size. A dielectric ceramic composition is obtained by the above process.

[0084] (Coating Process) Next, a binder such as polyvinyl butyral (PVB) resin, an organic solvent such as ethanol or toluene, and a plasticizer are added to the obtained dielectric ceramic composition and wet mixed. Using the obtained slurry, a ceramic green sheet 51 is coated on a substrate by, for example, a die coater method or a doctor blade method, and then dried. The substrate is, for example, a polyethylene terephthalate (PET) film. Figures illustrating the coating process are omitted.

[0085] (Internal Electrode Formation Process) Next, as illustrated in FIG. 7( a), a metal conductive paste containing an organic binder for forming internal electrodes is printed on the surface of a ceramic green sheet 51 by screen printing, gravure printing, or the like, to form an internal electrode pattern 52 that alternately leads to a pair of external electrodes with opposite polarities. Ceramic particles are added to the metal conductive paste as a co-material. The main component of the ceramic particles is not particularly limited, but is preferably the same as the main ceramic component of the dielectric layer 11. For example, barium titanate having an average particle diameter of 50 nm or less may be uniformly dispersed.

[0086] Next, a binder such as an ethyl cellulose-based binder and an organic solvent such as a terpineol-based binder are added to the dielectric ceramic composition obtained in the raw material powder preparation step, and the mixture is kneaded in a roll mill to obtain a dielectric pattern paste for the reverse pattern layer. As illustrated in Figure 7(a), a dielectric pattern paste is printed on a ceramic green sheet 51 in the peripheral area where the internal electrode pattern 52 is not printed, thereby arranging the dielectric pattern 53 and filling in the step with the internal electrode pattern 52. The ceramic green sheet 51 on which the internal electrode pattern 52 and the dielectric pattern 53 are printed is called a lamination unit.

[0087] 7(b), the lamination units are laminated so that the internal electrode layers 12 and the dielectric layers 11 are alternately arranged, and so that the edges of the internal electrode layers 12 are alternately exposed on both longitudinal end faces of the dielectric layers 11 and are alternately drawn out to a pair of external electrodes 20a, 20b having opposite polarities. For example, the number of laminated layers of the internal electrode pattern 52 is set to 100 to 1000.

[0088] 8, a predetermined number of cover sheets 54 (for example, 2 to 10 layers) are laminated on the top and bottom of the laminate in which the lamination units are stacked, and then thermocompression bonded. As an example, the above-mentioned dielectric ceramic composition can be used as the ceramic material for the cover sheets 54. Then, the laminate is cut to a predetermined chip size (for example, 1.0 mm x 0.5 mm).

[0089] (Firing step) The ceramic laminate thus obtained is 2 After binder removal treatment in an atmosphere, air atmosphere, etc., a metal paste that will become the base layer of the external electrodes 20a, 20b is applied by dipping, and the metal paste is then applied under an oxygen partial pressure of 10 -12 ~10 -9 The resulting mixture is fired in a reducing atmosphere at 1100 to 1300°C for 10 minutes to 2 hours at 1 atm. In this manner, the multilayer ceramic capacitor 100 is obtained. The firing process involves rapid temperature increase. The temperature increase rate in the firing process is, for example, 6000°C / h. This shortens the actual firing time and enables higher mass productivity.

[0090] (Annealing step) After that, oxygen partial pressure 10-12 ~10 -9 The dielectric layer 11 is annealed at 900 to 1150°C for 30 minutes to 2 hours in a reducing atmosphere of 100 atm, and then slowly cooled. The cooling rate is, for example, 200°C / h. In this manner, the main phase crystal grains 40 illustrated in FIG. 1 can be formed in at least a portion of the dielectric layer 11 in the capacitance region 14, and the first crystal grains 41 can also be formed.

[0091] (Reoxidation treatment step) Then, N 2 A reoxidation treatment may be carried out in a gas atmosphere at 600° C. to 1000° C.

[0092] (Plating Process) Thereafter, the underlayers of the external electrodes 20a, 20b are coated with a metal such as Cu, Ni, Sn, etc. by plating. Through the above processes, the multilayer ceramic capacitor 100 is completed.

[0093] According to the manufacturing method of this embodiment, it is possible to form the main phase crystal grains 40 illustrated in Fig. 1 and the first crystal grains 41 in at least a part of the dielectric layer 11 in the capacitance region 14. This makes it possible to achieve high reliability and high insulation resistance.

[0094] The direct current resistivity ρ (Ω·cm) of the multilayer ceramic capacitor is measured by the following method.

[0095] First, the DC current I (nA) is measured for the multilayer ceramic capacitor 100 that has undergone the firing, annealing, reoxidation, and plating processes. Next, the capacitance region 14 of the multilayer ceramic capacitor 100 is exposed by cutting or polishing the cross sections of lines A-A and B-B shown in FIGS. 4 and 5 , and the effective area of ​​the internal electrode layers 12 is calculated after the cross sections are polished to a smoothness comparable to a mirror finish, typically using diamond paste of 2 microns or less. The effective area S is calculated using the formula S = L × W × (N-1), where L is the length (X-axis direction) of the internal electrode layers 12 in the capacitance region 14 in FIG. 4 , N is the number of layers, and W is the width (Y-axis direction) of the internal electrode layers 12 in the capacitance region 14 in FIG. 5 . The thickness of each dielectric layer 11 is also measured, and the average thickness t is calculated. In this case, the DC resistivity ρ (Ω·cm) can be calculated by ρ=V / I×S / t, where V (V) is the DC voltage during measurement.

[0096] In the above embodiments, a multilayer ceramic capacitor has been described as an example of a multilayer ceramic electronic component, but the present invention is not limited to this. For example, other multilayer ceramic electronic components such as a varistor or a thermistor may also be used.

[0097] Example 1 Barium titanate powder having an average particle size of 150 nm was prepared. Gd 2 O 3 0.75 mol of TiO 2 2.0 mol of MnCO 3 1.5 mol of SiO 2 1.0 mol of Ba and 0.5 mol of MgO were added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.980.

[0098] A dielectric ceramic composition was mixed with ethanol, toluene, and PVB (polyvinyl butyral) resin to prepare a dielectric slurry. This slurry was then formed into ceramic green sheets using a die coater and dried. A metal conductive paste containing the main component metal of the internal electrode layer 12, co-materials, binder (ethyl cellulose), solvent, and other optional additives was prepared using a planetary ball mill and screen-printed onto ceramic green sheets. Eleven laminate units with the metal conductive paste printed on the ceramic green sheets were stacked, and cover sheets were laminated on the top and bottom of each. A laminate was then obtained by thermocompression bonding and cut into a predetermined shape. The resulting laminate was debindered in a N2 atmosphere, and a metal conductive paste containing a Ni-based metal filler, co-materials, binder, solvent, etc. was applied as a base layer to both end faces and each side of the laminate and dried. The metal conductive paste for the base layer was then fired simultaneously with the laminate at 1300°C in a reducing atmosphere to obtain a sintered body. The temperature rise rate was 6000°C / h. The resulting sintered body had dimensions of 0.6 mm in length, 0.3 mm in width, and 0.3 mm in height. Annealing was then performed at 900 to 1150°C for 1 hour. A reoxidation treatment was then performed at 950°C. A plating treatment was then performed to form a Cu plating layer, a Ni plating layer, and a Sn plating layer on the surface of the underlayer, yielding a multilayer ceramic capacitor 100. The average thickness of the dielectric layer 11 was 2.0 μm.

[0099] Example 2 In Example 2, Gd 2 O 3 0.75 mol of TiO 2 4.0 mol of MnCO 3 1.5 mol of SiO 2 1.0 mol of Ba was added, and 0.5 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.962. The firing temperature was 1250°C. The annealing time was 1 hour. The other conditions were the same as in Example 1.

[0100] Example 3 In Example 3, Gd 2 O 30.75 mol of TiO 2 4.0 mol of MnCO 3 1.5 mol of SiO 2 1.0 mol of Ba was added, and 0.5 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.962. The firing temperature was 1250°C. The annealing time was 0.5 hours. The other conditions were the same as in Example 1.

[0101] Example 4 In Example 4, Gd 2 O 3 0.75 mol of TiO 2 4.0 mol of MnCO 3 1.5 mol of SiO 2 1.0 mol of Ba was added, and 0.5 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.962. The firing temperature was 1250°C. The annealing time was 2 hours. The other conditions were the same as in Example 1.

[0102] Example 5 In Example 5, Gd 2 O 3 0.75 mol of TiO 2 6.0 mol of MnCO 3 1.5 mol of SiO 2 1.0 mol of Ba was added, and 0.5 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.943. The firing temperature was 1200°C. The annealing time was 1 hour. The other conditions were the same as in Example 1.

[0103] Example 6 In Example 6, Gd 2 O 3 0.75 mol of TiO 2 4.0 mol of MnCO 3 1.5 mol of SiO 21.0 mol of Ba was added, and 0.2 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.962. The firing temperature was 1280°C. The annealing time was 1 hour. The other conditions were the same as in Example 1.

[0104] Example 7 In Example 7, Gd 2 O 3 0.75 mol of TiO 2 4.0 mol of MnCO 3 1.5 mol of SiO 2 1.0 mol of Ba was added, and 1.0 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.962. The firing temperature was 1250°C. The annealing time was 1 hour. The other conditions were the same as in Example 1.

[0105] Example 8 In Example 8, Gd 2 O 3 0.75 mol of TiO 2 4.0 mol of MnCO 3 1.5 mol of SiO 2 1.0 mol of Ba was added, and 2.0 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.962. The firing temperature was 1250°C. The annealing time was 1 hour. The other conditions were the same as in Example 1.

[0106] Example 9 In Example 9, Gd 2 O 3 0.75 mol of TiO 2 4.0 mol of MnCO 3 1.5 mol of SiO 2 0.2 mol of Ba was added, and 0.5 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.962. The firing temperature was 1300°C. The annealing time was 1 hour. The other conditions were the same as in Example 1.

[0107] Example 10 In Example 10, Gd 2 O 3 0.75 mol of TiO 2 4.0 mol of MnCO 3 1.5 mol of SiO 2 0.5 mol of Ba was added, and 0.5 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.962. The firing temperature was 1300°C. The annealing time was 1 hour. The other conditions were the same as in Example 1.

[0108] Example 11 In Example 11, Gd 2 O 3 0.75 mol of TiO 2 4.0 mol of MnCO 3 1.5 mol of SiO 2 2.0 mol of Ba was added, and 0.5 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.962. The firing temperature was 1200°C. The annealing time was 1 hour. The other conditions were the same as in Example 1.

[0109] Example 12 In Example 12, Gd 2 O 3 0.75 mol of TiO 2 4.0 mol of MnCO 3 5.0 mol of SiO 2 0.5 mol of Ba was added, and 0.5 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.962. The firing temperature was 1300°C. The annealing time was 0.5 hours. The other conditions were the same as in Example 1.

[0110] Example 13 In Example 13, Gd was added to 100 mol of barium titanate powder. 2 O 3 0.75 mol of TiO 2 4.0 mol of MnCO 3 0.2 mol of SiO 20.5 mol of Ba was added, and 0.5 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.962. The firing temperature was 1300°C. The annealing time was 2 hours. The other conditions were the same as in Example 1.

[0111] Comparative Example 1 In Comparative Example 1, Gd 2 O 3 0.75 mol of TiO 2 1.0 mol of MnCO 3 1.5 mol of SiO 2 1.0 mol of Ba was added, and 0.5 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.990. The firing temperature was 1320°C. The annealing time was 2 hours. The other conditions were the same as in Example 1.

[0112] Comparative Example 2 In Comparative Example 2, Gd 2 O 3 0.75 mol of TiO 2 8.0 mol of MnCO 3 1.5 mol of SiO 2 1.0 mol of Ba was added, and 0.5 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.926. The firing temperature was 1160°C. The annealing time was 1 hour. The other conditions were the same as in Example 1.

[0113] Comparative Example 3 In Comparative Example 3, Gd 2 O 3 0.75 mol of TiO 2 4.0 mol of MnCO 3 1.5 mol of SiO 2 1.0 mol of Ba was added, and 0.05 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.962. The firing temperature was 1300°C. The annealing time was 1 hour. The other conditions were the same as in Example 1.

[0114] Comparative Example 4 In Comparative Example 4, Gd 2 O 3 0.75 mol of TiO 2 4.0 mol of MnCO 3 1.5 mol of SiO 2 1.0 mol of Ba was added, and 5.0 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.962. The firing temperature was 1200°C. The annealing time was 1 hour. The other conditions were the same as in Example 1.

[0115] Comparative Example 5 In Comparative Example 5, Gd 2 O 3 0.75 mol of TiO 2 4.0 mol of MnCO 3 1.5 mol of SiO 2 1.0 mol of Ba was added, and 0.5 mol of MgO was added to obtain a dielectric ceramic composition. The Ba / Ti element ratio was 0.962. The firing temperature was 1250°C. The annealing time was 0 hours. In other words, no annealing treatment was performed. The other conditions were the same as in Example 1.

[0116] The conditions for Examples 1 to 13 and Comparative Examples 1 to 5 are shown in Table 1.

[0117] For each of the multilayer ceramic capacitors of Examples 1 to 13 and Comparative Examples 1 to 5, a direct current I was measured at 150°C with an insulation resistance meter while applying 60 V for 30 seconds, and the resistivity ρ was calculated. The presence or absence of first crystal particles in the dielectric layers satisfying the following conditions was confirmed: 5.00≦Ti / Ba element ratio a≦7.00 and 0.50≦Mg / Ba element ratio b≦1.50. The Ti / Ba element ratio a, Mg / Ba element ratio b, Mn / Ba element ratio g, and Ni / Ba element ratio h of the first crystal particles were also measured. Furthermore, the presence or absence of second crystal particles in which the elemental ratios of titanium, magnesium, manganese, and nickel relative to barium were higher than those of the surrounding main phase crystal particles made of barium titanate and the elemental ratios of titanium, magnesium, manganese, and nickel relative to barium were lower than those of the first crystal particles was confirmed. Furthermore, the Ti / Ba element ratio c, Mg / Ba element ratio d, Mn / Ba element ratio e, and Ni / Ba element ratio f in the second crystal particles were measured. The results are shown in Table 2.

[0118] In Example 1, first crystal particles were observed. In the first crystal particles, the Ti / Ba element ratio a was 5.32, the Mg / Ba element ratio b was 1.00, the Mn / Ba element ratio g was 2.28, and the Ni / Ba element ratio h was 1.76. In addition, second crystal particles were observed. In the second crystal particles, the Ti / Ba element ratio c was 1.62, the Mg / Ba element ratio d was 0.14, the Mn / Ba element ratio e was 0.14, and the Ni / Ba element ratio f was 0.18. The resistivity ρ was 2.9×10 11 The value was Ω·cm.

[0119] In Example 2, first crystal particles were observed. In the first crystal particles, the Ti / Ba element ratio a was 5.60, the Mg / Ba element ratio b was 1.11, the Mn / Ba element ratio g was 2.85, and the Ni / Ba element ratio h was 2.02. In addition, second crystal particles were observed. In the second crystal particles, the Ti / Ba element ratio c was 2.16, the Mg / Ba element ratio d was 0.13, the Mn / Ba element ratio e was 0.12, and the Ni / Ba element ratio f was 0.20. The resistivity ρ was 9.5×10 11 The value was Ω·cm.

[0120] In Example 3, first crystal particles were observed. In the first crystal particles, the Ti / Ba element ratio a was 5.66, the Mg / Ba element ratio b was 1.14, the Mn / Ba element ratio g was 3.42, and the Ni / Ba element ratio h was 1.01. In addition, second crystal particles were observed. In the second crystal particles, the Ti / Ba element ratio c was 2.31, the Mg / Ba element ratio d was 0.12, the Mn / Ba element ratio e was 0.03, and the Ni / Ba element ratio f was 0.37. The resistivity ρ was 2.1×10 11 The value was Ω·cm.

[0121] In Example 4, first crystal particles were observed. In the first crystal particles, the Ti / Ba element ratio a was 5.71, the Mg / Ba element ratio b was 1.10, the Mn / Ba element ratio g was 1.71, and the Ni / Ba element ratio h was 3.03. Furthermore, no second crystal particles were observed. The resistivity ρ was 4.1×10 10 The value was Ω·cm.

[0122] In Example 5, first crystal particles were observed. In the first crystal particles, the Ti / Ba element ratio a was 6.85, the Mg / Ba element ratio b was 1.08, the Mn / Ba element ratio g was 0.15, and the Ni / Ba element ratio h was 2.10. In addition, second crystal particles were observed. In the second crystal particles, the Ti / Ba element ratio c was 3.23, the Mg / Ba element ratio d was 0.11, the Mn / Ba element ratio e was 0.12, and the Ni / Ba element ratio f was 0.19. The resistivity ρ was 1.5×10 11 The value was Ω·cm.

[0123] In Example 6, first crystal particles were observed. In the first crystal particles, the Ti / Ba element ratio a was 5.82, the Mg / Ba element ratio b was 0.54, the Mn / Ba element ratio g was 2.74, and the Ni / Ba element ratio h was 2.04. In addition, second crystal particles were observed. In the second crystal particles, the Ti / Ba element ratio c was 2.20, the Mg / Ba element ratio d was 0.03, the Mn / Ba element ratio e was 0.12, and the Ni / Ba element ratio f was 0.16. The resistivity ρ was 2.0×10 11The value was Ω·cm.

[0124] In Example 7, first crystal particles were observed. In the first crystal particles, the Ti / Ba element ratio a was 5.71, the Mg / Ba element ratio b was 1.21, the Mn / Ba element ratio g was 2.72, and the Ni / Ba element ratio h was 2.02. In addition, second crystal particles were observed. In the second crystal particles, the Ti / Ba element ratio c was 2.09, the Mg / Ba element ratio d was 0.16, the Mn / Ba element ratio e was 0.11, and the Ni / Ba element ratio f was 0.24. The resistivity ρ was 6.6×10 11 The value was Ω·cm.

[0125] In Example 8, first crystal particles were observed. In the first crystal particles, the Ti / Ba element ratio a was 5.60, the Mg / Ba element ratio b was 1.44, the Mn / Ba element ratio g was 2.91, and the Ni / Ba element ratio h was 1.94. In addition, second crystal particles were observed. In the second crystal particles, the Ti / Ba element ratio c was 2.03, the Mg / Ba element ratio d was 0.29, the Mn / Ba element ratio e was 0.11, and the Ni / Ba element ratio f was 0.24. The resistivity ρ was 2.9×10 11 The value was Ω·cm.

[0126] In Example 9, first crystal particles were observed. In the first crystal particles, the Ti / Ba element ratio a was 5.15, the Mg / Ba element ratio b was 0.78, the Mn / Ba element ratio g was 2.88, and the Ni / Ba element ratio h was 1.96. In addition, second crystal particles were observed. In the second crystal particles, the Ti / Ba element ratio c was 2.18, the Mg / Ba element ratio d was 0.12, the Mn / Ba element ratio e was 0.12, and the Ni / Ba element ratio f was 0.22. The resistivity ρ was 5.1×10 11 The value was Ω·cm.

[0127] In Example 10, first crystal particles were observed. In the first crystal particles, the Ti / Ba element ratio a was 5.26, the Mg / Ba element ratio b was 0.92, the Mn / Ba element ratio g was 2.89, and the Ni / Ba element ratio h was 2.00. In addition, second crystal particles were observed. In the second crystal particles, the Ti / Ba element ratio c was 2.24, the Mg / Ba element ratio d was 0.12, the Mn / Ba element ratio e was 0.12, and the Ni / Ba element ratio f was 0.22. The resistivity ρ was 4.9×10 11 The value was Ω·cm.

[0128] In Example 11, first crystal particles were observed. In the first crystal particles, the Ti / Ba element ratio a was 6.72, the Mg / Ba element ratio b was 1.33, the Mn / Ba element ratio g was 1.91, and the Ni / Ba element ratio h was 1.98. In addition, second crystal particles were observed. In the second crystal particles, the Ti / Ba element ratio c was 2.22, the Mg / Ba element ratio d was 0.12, the Mn / Ba element ratio e was 0.12, and the Ni / Ba element ratio f was 0.22. The resistivity ρ was 3.9×10 11 The value was Ω·cm.

[0129] In Example 12, first crystal particles were observed. In the first crystal particles, the Ti / Ba element ratio a was 5.38, the Mg / Ba element ratio b was 0.92, the Mn / Ba element ratio g was 4.13, and the Ni / Ba element ratio h was 0.07. In addition, second crystal particles were observed. In the second crystal particles, the Ti / Ba element ratio c was 2.76, the Mg / Ba element ratio d was 0.12, the Mn / Ba element ratio e was 0.02, and the Ni / Ba element ratio f was 0.32. The resistivity ρ was 2.3×10 10 The value was Ω·cm.

[0130] In Example 13, first crystal particles were observed. In the first crystal particles, the Ti / Ba element ratio a was 5.43, the Mg / Ba element ratio b was 0.97, the Mn / Ba element ratio g was 0.05, and the Ni / Ba element ratio h was 4.12. In addition, second crystal particles were observed. In the second crystal particles, the Ti / Ba element ratio c was 1.83, the Mg / Ba element ratio d was 0.13, the Mn / Ba element ratio e was 0.32, and the Ni / Ba element ratio f was 0.05. The resistivity ρ was 2.4×10 10 The value was Ω·cm.

[0131] In Comparative Example 1, neither the first crystal grains nor the second crystal grains were observed. The resistivity ρ was 4.4×10 9 The value was Ω·cm.

[0132] In Comparative Example 2, no first crystal particles were observed, but second crystal particles were observed. In the second crystal particles, the Ti / Ba element ratio c was 3.05, the Mg / Ba element ratio d was 0.11, the Mn / Ba element ratio e was 0.11, and the Ni / Ba element ratio f was 0.18. The resistivity ρ was 1.3×10 9 The value was Ω·cm.

[0133] In Comparative Example 3, no first crystal particles were observed, but second crystal particles were observed. In the second crystal particles, the Ti / Ba element ratio c was 2.37, the Mg / Ba element ratio d was 0.00, the Mn / Ba element ratio e was 0.35, and the Ni / Ba element ratio f was 0.38. The resistivity ρ was 5.8×10 9 The value was Ω·cm.

[0134] In Comparative Example 4, no first crystal particles were observed, but second crystal particles were observed. In the second crystal particles, the Ti / Ba element ratio c was 2.09, the Mg / Ba element ratio d was 0.31, the Mn / Ba element ratio e was 0.11, and the Ni / Ba element ratio f was 0.22. The resistivity ρ was 1.8×10 9 The value was Ω·cm.

[0135] In Comparative Example 5, no first crystal particles were observed, but second crystal particles were observed. In the second crystal particles, the Ti / Ba element ratio c was 2.16, the Mg / Ba element ratio d was 0.13, the Mn / Ba element ratio e was 0.12, and the Ni / Ba element ratio f was 0.20. The resistivity ρ was 8.0×10 9 The value was Ω·cm.

[0136] The results of Examples 1 to 13 and Comparative Examples 1 to 5 are shown in Table 2.

[0137] As shown in Table 2, in Examples 1 to 13, the resistivity ρ (Ω·cm) was 10 10 It was confirmed that a high insulation resistance was achieved, which is on the order of 1000 kJ / cm. This is believed to be due to the formation of first crystal grains in addition to the main phase crystal grains.

[0138] The resistivity of Examples 1 to 3 and 5 to 11 was higher than that of Examples 4, 12, and 13. This is thought to be because, in Examples 1 to 3 and 5 to 11, second crystal particles were confirmed in addition to the first crystal particles, and the second crystal particles satisfied the following conditions: 1.50≦Ti / Ba element ratio c≦3.50, 0.03≦Mg / Ba element ratio d≦0.30, 0.03≦Mn / Ba element ratio e≦0.30, and 0.03≦Ni / Ba element ratio f≦0.40.

[0139] In addition, for Examples 1 to 13, composition evaluation by EDS was performed on the main phase crystal grains contained in the dielectric layers, and it was confirmed that the main phase crystal grains had a core-shell structure.

[0140] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and changes are possible within the scope of the gist of the present invention as described in the claims.

[0141] REFERENCE SIGNS LIST 10 laminated chip 11 dielectric layer 12 internal electrode layer 13 cover layer 14 capacitance region 15 end margin 16 side margin 20a, 20b external electrode 40 main phase crystal grain 41 first crystal grain 42 second crystal grain 43 third crystal grain 44 gap 51 ceramic green sheet 52 internal electrode pattern 53 dielectric pattern 54 cover sheet 55 side margin portion 100 multilayer ceramic capacitor

Claims

1. A dielectric ceramic composition comprising: a main phase containing barium titanate having a perovskite structure; first crystal particles containing barium, titanium, and magnesium, wherein, when the atomic ratio of titanium to the barium content is a, and the atomic ratio of magnesium to the barium content is b, the following relationships are satisfied: 5.00≦a≦7.00, and 0.50≦b≦1.50; and second crystal particles containing barium, titanium, magnesium, manganese, and nickel, wherein, when the atomic ratio of titanium to the barium content is c, the atomic ratio of magnesium to the barium content is d, the atomic ratio of manganese to the barium content is e, and the atomic ratio of nickel to the barium content is f, the following relationships are satisfied: 1.50≦c≦3.50, 0.03≦d≦0.30, 0.03≦e≦0.30, and 0.03≦f≦0.

40.

2. The dielectric ceramic composition according to claim 1, wherein the first crystal particles further contain manganese and nickel, and in the first crystal particles, when the elemental ratio of manganese to the barium content is g and the elemental ratio of nickel to the barium content is h, the relationship 0.10≦g≦4.00 and 0.10≦h≦4.00 are satisfied.

3. The dielectric ceramic composition of claim 1, further comprising third crystalline particles comprising at least one of silicate, enstatite, barium magnesium silicate, or fresnoite.

4. The dielectric ceramic composition according to claim 1, wherein the first crystal grains and the second crystal grains are located at grain boundaries of the main phase.

5. The dielectric ceramic composition according to claim 1, wherein the first crystal grains and the second crystal grains are located at grain boundary triple junctions of the main phase.

6. The dielectric ceramic composition according to claim 3, wherein the third crystal grains are located at the grain boundaries of the main phase.

7. The dielectric ceramic composition according to claim 3, wherein the third crystal grains are located at the grain boundary triple points of the main phase.

8. The dielectric ceramic composition according to claim 1, wherein the main phase has a core portion and a shell portion covering the core portion.

9. The dielectric ceramic composition according to claim 8, wherein said shell portion contains a rare earth element.

10. A dielectric ceramic composition according to claim 1, wherein the atomic ratio of barium to titanium is 0.940 or more and 0.980 or less, the atomic ratio of gadolinium to titanium is 0.005 or more and 0.05 or less, and the atomic ratio of magnesium to titanium is 0.002 or more and 0.02 or less.

11. A dielectric ceramic composition comprising: a main phase having a perovskite structure, containing barium titanate, and having a core portion and a shell portion covering said core portion; and first crystal particles containing barium, titanium, and magnesium, wherein, when the elemental ratio of titanium to the barium content is a and the elemental ratio of magnesium to the barium content is b, 5.00≦a≦7.00 and 0.50≦b≦1.50 are satisfied.

12. The dielectric ceramic composition according to claim 11, wherein the first crystal particles further contain manganese and nickel, and in the first crystal particles, when the elemental ratio of manganese to the barium content is g and the elemental ratio of nickel to the barium content is h, 0.10≦g≦4.00 and 0.10≦h≦4.00 are satisfied.

13. A multilayer ceramic electronic component comprising: a plurality of dielectric layers containing the dielectric ceramic composition according to claim 1; a plurality of internal electrodes opposed to each other with the plurality of dielectric layers interposed therebetween; and an external electrode electrically connected to the plurality of internal electrodes.

Citation Information

Patent Citations

  • Laminated ceramic capacitor and method of manufacturing it

    JP2001230149A

  • Dielectric composition and laminated ceramic electronic component

    JP2022181544A

  • Multilayer ceramic capacitor and method for production thereof

    WO2008038722A1

  • Laminated ceramic capacitor

    WO2014002302A1

Cited By

  • Mg-mo synergistic anti-reduction x7r barium titanate ceramic and preparation method thereof

    CN122916653A