Prepreg, metal-clad laminate, and printed wiring board

The integration of a thermosetting resin composition with a specific glass cloth composition in prepregs addresses the challenges of moldability and thermal expansion, enhancing drilling accuracy and producing more precise printed wiring boards.

WO2024203311A1PCT designated stage expired Publication Date: 2024-10-03PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009674
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-13
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing prepregs and printed wiring boards face challenges in achieving good moldability, low coefficient of thermal expansion, and accurate hole positioning during drilling, with limitations in chemical composition changes for glass cloth impregnation.

Method used

A prepreg comprising a thermosetting resin composition with a high content of inorganic filler and a specific glass cloth composition, including SiO2, ZnO, Al2O3, and MgO, integrated with a thermosetting resin composition to enhance moldability, reduce thermal expansion, and improve drilling accuracy.

Benefits of technology

The solution achieves good moldability, low coefficient of thermal expansion, and improved hole positioning accuracy, enabling the production of thinner, lighter, and more precise metal-clad laminates and printed wiring boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009674_03102024_PF_FP_ABST
    Figure JP2024009674_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure addresses the problem of providing a prepreg that can have a low thermal expansion coefficient while obtaining fine moldability, and that can increase bore position accuracy in drilling. A prepreg (1) comprises: a thermosetting resin composition (2) or a semi-cured product of the thermosetting resin composition (2); and a glass cloth (3) integrated with the thermosetting resin composition (2) or the semi-cured product. The thermosetting resin composition (2) contains a thermosetting compound (A) and an inorganic filler (B). The contained amount of the inorganic filler (B) is 90-210 parts by mass with respect to 100 parts by mass of the thermosetting compound (A). The glass cloth (3) contains 59 mass% or more of SiO2, 1.0-8.0 mass% of ZnO, 15-20 mass% of Al2O3, 2.0 mass% or more of B2O3, and 2.0 mass% or more of MgO.
Need to check novelty before this filing date? Find Prior Art

Description

Prepregs, metal-clad laminates, and printed wiring boards

[0001] The present disclosure relates generally to prepregs, metal-clad laminates, and printed wiring boards, and more particularly to prepregs, metal-clad laminates, and printed wiring boards comprising a thermosetting resin composition.

[0002] Patent Document 1 discloses a glass sheet material. This glass sheet material is used for compounding with an organic resin material to form an organic resin composite material. This glass sheet material is made of glass fiber and processed into a glass cloth or nonwoven fabric.

[0003] Here, the glass fiber is made of a composition for glass fiber. The composition for glass fiber contains SiO 2 in terms of mass percentage of oxide. 2 55 to 70%, Al 2 O 3 15-25%, MgO 3-13%, CaO 0-3%, B 2 O 3 0.5 to 6%, MgO + CaO + SrO + BaO + ZnO 5 to 15%, SiO 2 +Al 2 O 3 78 to 88%, Al 2 O 3 + 23 to 32% MgO, TiO 2 0.1 to 5%, ZrO 0 to 1%, Li 2 O + Na 2 O+K 2 Contains 0 to 1% O.

[0004] Paragraph

[0027] of Patent Document 1 discloses that glass cloth is impregnated with resin and processed into a prepreg. According to this disclosure, warping of the prepreg can be suppressed by the effect of the MgO component. It also discloses that an increase in the content of the MgO component increases the linear thermal expansion coefficient of the glass.

[0005] On the other hand, in paragraph

[0025] of Patent Document 1, SiO 2 It is disclosed that an increase in the content of the component increases the wear of the drill when drilling holes in a printed wiring board.

[0006] However, Patent Document 1 does not disclose any means for improving the positional accuracy of holes formed by drilling. In particular, when attempting to improve the positional accuracy of holes formed by drilling, with the premise of obtaining good formability while reducing the thermal expansion coefficient, there is a limit to what can be achieved by simply changing the chemical composition of the glass cloth. In other words, some kind of ingenuity is required with respect to the composition impregnated into the glass cloth.

[0007] JP 2011-105554 A

[0008] An object of the present disclosure is to provide a prepreg, a metal-clad laminate, and a printed wiring board that can achieve good moldability while reducing the thermal expansion coefficient and improving the hole position accuracy by drilling.

[0009] A prepreg according to one aspect of the present disclosure includes a thermosetting resin composition or a semi-cured product of the thermosetting resin composition, and glass cloth integrated with the thermosetting resin composition or the semi-cured product. The thermosetting resin composition includes a thermosetting compound (A) and an inorganic filler (B). The content of the inorganic filler (B) is 90 parts by mass or more and 210 parts by mass or less per 100 parts by mass of the thermosetting compound (A). The glass cloth is made of SiO 2 59% by mass or more, ZnO 1.0% by mass or more and 8.0% by mass or less, Al 2 O 3 15% by mass or more and 20% by mass or less, B 2 O 3 and 2.0 mass % or more of MgO.

[0010] A metal-clad laminate according to one embodiment of the present disclosure includes an insulating layer containing a cured product of the prepreg, and a metal layer.

[0011] A printed wiring board according to one aspect of the present disclosure includes an insulating layer containing a cured product of the prepreg, and conductor wiring.

[0012] Fig. 1 is a schematic cross-sectional view showing a prepreg according to the present embodiment, Fig. 2 is a schematic cross-sectional view showing a metal-clad laminate according to the present embodiment, and Fig. 3 is a schematic cross-sectional view showing a printed wiring board according to the present embodiment.

[0013] 1. Overview As shown in FIG. 1 , a prepreg 1 according to this embodiment includes a thermosetting resin composition 2 or a semi-cured product of the thermosetting resin composition 2, and a glass cloth 3 integrated with the thermosetting resin composition 2 or the semi-cured product.

[0014] The thermosetting resin composition 2 contains a thermosetting compound (A) and an inorganic filler (B).

[0015] The content of the inorganic filler (B) is 90 parts by mass or more and 210 parts by mass or less relative to 100 parts by mass of the thermosetting compound (A). When the content of the inorganic filler (B) is 210 parts by mass or less, good moldability can be obtained when the thermosetting resin composition 2 is impregnated into the glass cloth 3. Here, it can be said that the smaller the unimpregnated portion (the portion of the glass cloth 3 that is not impregnated with the thermosetting resin composition 2), the better the moldability.

[0016] The glass cloth 3 is SiO 2 59% by mass or more, ZnO 1.0% by mass or more and 8.0% by mass or less, Al 2 O 3 15% by mass or more and 20% by mass or less, B 2 O 3 and 2.0 mass % or more of MgO.

[0017] In particular, the glass cloth 3 is made of SiO 2 By including 59% by mass or more of the prepreg 1, it is possible to reduce the coefficient of thermal expansion (CTE) of the metal-clad laminate 10 formed from the prepreg 1. Here, the coefficient of thermal expansion mainly refers to the coefficient of linear expansion along a direction perpendicular to the Z-axis direction (for example, the Y-axis direction) (see FIG. 2).

[0018] Furthermore, when the glass cloth 3 contains 1.0 mass % or more and 8.0 mass % or less of ZnO, the thermal expansion coefficient of the metal-clad laminate 10 can be maintained low, while the hole position accuracy in drilling can be improved.

[0019] Therefore, according to this embodiment, it is possible to obtain good moldability while reducing the thermal expansion coefficient and improving the accuracy of hole positioning by drilling.

[0020] 2. Details The prepreg 1, metal-clad laminate 10, and printed wiring board 100 according to this embodiment will be described below with reference to FIGS. 1 to 3. Each figure is a schematic diagram, and the ratios of the size and thickness of each component in each figure do not necessarily reflect the actual dimensional ratios. The arrows indicating each direction in each figure are not intended to define the direction of use of the prepreg 1, metal-clad laminate 10, and printed wiring board 100; they are merely shown to facilitate understanding of the description and have no substance. The X-axis, Y-axis, and Z-axis directions are mutually orthogonal. The Z-axis direction is the thickness direction of the prepreg 1, metal-clad laminate 10, and printed wiring board 100.

[0021] 1, the prepreg 1 according to this embodiment is an adhesive sheet that extends in the X-axis direction and the Y-axis direction and has a thickness in the Z-axis direction. The prepreg 1 can be used as a material for a metal-clad laminate 10 and a printed wiring board 100.

[0022] The prepreg 1 according to this embodiment comprises a thermosetting resin composition 2 or a semi-cured product of the thermosetting resin composition 2, and a glass cloth 3 integrated with the thermosetting resin composition 2 or the semi-cured product. Here, the semi-cured product refers to a substance in the B stage. The B stage is an intermediate stage in the curing reaction of the thermosetting resin composition 2. In other words, the B stage is a stage between the A stage, which is the initial stage of the curing reaction, and the C stage, which is the final stage of the curing reaction.

[0023] The average thickness of the prepreg 1 is preferably 45 μm or more, more preferably 50 μm or more, and even more preferably 60 μm or more. On the other hand, the average thickness of the prepreg 1 is preferably 200 μm or less, more preferably 195 μm or less, and even more preferably 190 μm or less. If the thickness is within the above range, good thickness accuracy can be obtained.

[0024] <Thermosetting Resin Composition> The thermosetting resin composition 2 includes a thermosetting compound (A) and an inorganic filler (B). The thermosetting resin composition 2 may further include at least one of a polymer (C), core-shell rubber particles (D), and a curing accelerator.

[0025] <<Thermosetting Compound (A)>> The thermosetting compound (A) is not particularly limited, but preferably contains one or more compounds selected from the group consisting of epoxy resins, phenolic resins, cyanate resins, melamine resins, imide resins, and dicyandiamide, thereby imparting characteristics to the prepreg 1 according to the various compounds.

[0026] Preferably, the thermosetting compound (A) contains an epoxy resin, which is excellent in mechanical strength, heat resistance, electrical properties, chemical resistance, adhesiveness, and the like.

[0027] When the thermosetting compound (A) contains an epoxy resin, the content of the epoxy resin is 50% by mass or more, preferably 56% by mass or more, and more preferably 58% by mass or more, based on the total amount of the thermosetting compound (A). By having the epoxy resin content of 50% by mass or more, the glass transition temperature (Tg) of the cured product of the thermosetting resin composition 2 can be increased.

[0028] On the other hand, the content of the epoxy resin is 70 mass % or less, preferably 64 mass % or less, and more preferably 62 mass % or less, based on the total amount of the thermosetting compound (A). By making the content of the epoxy resin 70 mass % or less, the moisture absorption rate of the cured product of the thermosetting resin composition 2 can be reduced.

[0029] Preferably, the thermosetting compound (A) contains an epoxy resin and further contains a phenolic resin. The phenolic resin can function as a curing agent for the epoxy resin. The phenolic resin has excellent processability, heat resistance, durability, etc.

[0030] When the thermosetting compound (A) contains an epoxy resin and a phenolic resin, the content of the phenolic resin is 30% by mass or more, preferably 36% by mass or more, and more preferably 38% by mass or more, based on the total amount of the thermosetting compound (A). By having the content of the phenolic resin be 30% by mass or more, the glass transition temperature (Tg) of the cured product of the thermosetting resin composition 2 can be increased.

[0031] On the other hand, the content of the phenolic resin is 50 mass % or less, preferably 44 mass % or less, and more preferably 42 mass % or less, based on the total amount of the thermosetting compound (A). By making the content of the phenolic resin 50 mass % or less, the moisture absorption rate of the cured product of the thermosetting resin composition 2 can be reduced.

[0032] <Inorganic Filler (B)> The inorganic filler (B) is not particularly limited, but preferably contains one or more particles selected from the group consisting of zinc molybdate particles, silica particles, aluminum hydroxide particles, talc particles, calcium molybdate particles, magnesium hydroxide particles, and boehmite particles. This allows the prepreg 1 to be endowed with characteristics corresponding to the various particles. In particular, among the particles listed above, it is preferable that the inorganic filler (B) contains only silica particles and zinc molybdate particles. This further increases the hole position accuracy achieved by drilling.

[0033] The content of the inorganic filler (B) is 90 parts by mass or more, preferably 100 parts by mass or more, more preferably 110 parts by mass or more, per 100 parts by mass of the thermosetting compound (A). If the content of the inorganic filler (B) is less than 90 parts by mass, the thermal expansion coefficient of the metal-clad laminate 10 formed from the prepreg 1 may be high. Also, the thickness accuracy of the metal-clad laminate 10 formed from the prepreg 1 may be low.

[0034] On the other hand, the content of the inorganic filler (B) is 210 parts by mass or less, preferably 200 parts by mass or less, more preferably 190 parts by mass or less, per 100 parts by mass of the thermosetting compound (A). If the content of the inorganic filler (B) exceeds 210 parts by mass, moldability may be deteriorated.

[0035] When the inorganic filler (B) contains silica particles, the content of the silica particles is 30 parts by mass or more, preferably 35 parts by mass or more, and more preferably 40 parts by mass or more, per 100 parts by mass of the thermosetting compound (A).

[0036] On the other hand, the content of the silica particles is 110 parts by mass or less, preferably 105 parts by mass or less, and more preferably 100 parts by mass or less, per 100 parts by mass of the thermosetting compound (A).

[0037] When the inorganic filler (B) contains talc particles, the content of the talc particles is 1 part by mass or more, preferably 5 parts by mass or more, and more preferably 10 parts by mass or more, per 100 parts by mass of the thermosetting compound (A).

[0038] On the other hand, the content of the talc particles is 30 parts by mass or less, preferably 25 parts by mass or less, and more preferably 20 parts by mass or less, based on 100 parts by mass of the thermosetting compound (A).

[0039] When the inorganic filler (B) contains zinc molybdate particles, the content of the zinc molybdate particles is 1 part by mass or more, preferably 2 parts by mass or more, and more preferably 3 parts by mass or more, per 100 parts by mass of the thermosetting compound (A).

[0040] On the other hand, the content of the zinc molybdate particles is 25 parts by mass or less, preferably 20 parts by mass or less, and more preferably 17 parts by mass or less, per 100 parts by mass of the thermosetting compound (A).

[0041] When the inorganic filler (B) contains aluminum hydroxide particles, the content of the aluminum hydroxide particles is 43 parts by mass or more, preferably 48 parts by mass or more, and more preferably 50 parts by mass or more, per 100 parts by mass of the thermosetting compound (A).

[0042] On the other hand, the content of the aluminum hydroxide particles is 105 parts by mass or less, preferably 95 parts by mass or less, and more preferably 90 parts by mass or less, per 100 parts by mass of the thermosetting compound (A).

[0043] The inorganic filler (B) preferably has an average particle size of 0.1 μm or more. In this specification, the term "average particle size" refers to the particle size at 50% of the integrated value in the particle size distribution determined by a laser diffraction / scattering method (D50).

[0044] On the other hand, the average particle size of the inorganic filler (B) is preferably 10 μm or less, more preferably 8 μm or less, and even more preferably 6 μm or less. When the average particle size of the inorganic filler (B) is 10 μm or less, the specific surface area of ​​the inorganic filler (B) increases, which leads to improved hole position accuracy in drilling.

[0045] <<High Molecular Weight Material (C)>> Preferably, the thermosetting resin composition 2 further contains a high molecular weight material (C). The weight average molecular weight of the high molecular weight material (C) is 100,000 or more, preferably 150,000 or more, and more preferably 200,000 or more. On the other hand, the weight average molecular weight of the high molecular weight material (C) is preferably 1,000,000 or less, and more preferably 900,000 or less.

[0046] The polymer (C) is preferably a copolymer, but may also be a homopolymer. The monomers constituting the copolymer and homopolymer are not particularly limited, and examples thereof include acrylic acid esters and methacrylic acid esters.

[0047] By further including the polymer (C) in the thermosetting resin composition 2, the coefficient of thermal expansion can be further reduced. Furthermore, the thickness accuracy of the metal-clad laminate 10 formed from the prepreg 1 can be improved.

[0048] Preferably, the polymer (C) contains an acrylic monomer copolymer. This allows the thermal expansion coefficient to be further reduced compared to when the polymer (C) does not contain an acrylic monomer copolymer. Furthermore, the thickness accuracy of the metal-clad laminate 10 can be improved.

[0049] When the polymer (C) contains an acrylic monomer copolymer, the content of the acrylic monomer copolymer is preferably 5 parts by mass or more, more preferably 7 parts by mass or more, and even more preferably 9 parts by mass or more, relative to 100 parts by mass of the thermosetting compound (A). By having the content of the acrylic monomer copolymer be 5 parts by mass or more, the thermal expansion coefficient can be further reduced. Furthermore, the thickness accuracy of the metal-clad laminate 10 can also be improved.

[0050] On the other hand, the content of the acrylic monomer copolymer is preferably 20 parts by mass or less, more preferably 18 parts by mass or less, and even more preferably 16 parts by mass or less, per 100 parts by mass of the thermosetting compound (A). By ensuring that the content of the acrylic monomer copolymer is 20 parts by mass or less, the accuracy of hole positioning in drilling can be improved. Furthermore, a decrease in the adhesive strength of the cured product of the thermosetting resin composition 2 to the metal layer 5 can be suppressed.

[0051] <<Core-shell rubber particles (D)>> Preferably, the thermosetting resin composition 2 further contains core-shell rubber particles (D). The core-shell rubber particles (D) are rubber-like particles having a core and a shell surrounding the core. The core-shell rubber particles (D) are not particularly limited, but examples thereof include silicone-acrylic composite rubber, acrylic rubber, and butadiene rubber. In this embodiment, even if the weight-average molecular weight of the core and / or shell is 100,000 or more, the core-shell rubber particles (D) are not included in the polymer (C).

[0052] By including the core-shell rubber particles (D) in the thermosetting resin composition 2, the thermal expansion coefficient can be further reduced compared to when the thermosetting resin composition 2 does not include the core-shell rubber particles (D). Furthermore, the thickness accuracy of the metal-clad laminate 10 can be improved.

[0053] The thermosetting resin composition 2 preferably contains both the polymer (C) and the core-shell rubber particles (D), and more preferably contains both the acrylic monomer copolymer and the core-shell rubber particles (D).

[0054] When the thermosetting resin composition 2 contains both the acrylic monomer copolymer and the core-shell rubber particles (D), the mass ratio of the core-shell rubber particles (D) to the acrylic monomer copolymer is preferably 3:2 to 8:2, and more preferably 4:2 to 7:2. This makes it easier to obtain a synergistic effect of the acrylic monomer copolymer and the core-shell rubber particles (D) while maintaining high hole position accuracy in drilling.

[0055] The mass ratio of the core-shell rubber particles (D) to the acrylic monomer copolymer can be expressed as follows. That is, the total mass of the core-shell rubber particles (D) is preferably 1.5 times or more, more preferably 2 times or more, relative to the total mass of the acrylic monomer copolymer. When the total mass of the core-shell rubber particles (D) is 1.5 times or more, the impact resistance and thermal shock resistance of the cured product of the thermosetting resin composition 2 can be improved. On the other hand, the total mass of the core-shell rubber particles (D) is preferably 4 times or less, more preferably 3.5 times or less, relative to the total mass of the acrylic monomer copolymer. When the total mass of the core-shell rubber particles (D) is 4 times or less, the cured product of the thermosetting resin composition 2 can be prevented from experiencing a decrease in adhesive strength to the metal layer 5.

[0056] The average particle size of the core-shell rubber particles (D) is preferably 0.01 μm or more, more preferably 0.05 μm or more.

[0057] On the other hand, the average particle size of the core-shell rubber particles (D) is preferably 0.7 μm or less, more preferably 0.5 μm or less.

[0058] <<Curing Accelerator>> The curing accelerator is effective in accelerating the curing reaction of the thermosetting compound (A). The curing accelerator is not particularly limited, but examples thereof include 2-ethyl-4-methylimidazole. When the curing accelerator is contained in the thermosetting resin composition 2, the content of the curing accelerator is appropriately adjusted depending on the content of the thermosetting compound (A).

[0059] <Glass Cloth> The glass cloth 3 is a fabric woven using glass fiber threads as warp and weft. There are no particular limitations on the weaving method, but examples include plain weave and twill weave. As shown in Fig. 1 , the glass cloth 3 extends in the X-axis direction and the Y-axis direction and has a thickness in the Z-axis direction. The glass cloth 3 is used as a material for the prepreg 1.

[0060] The glass cloth 3 is composed of SiO 2 59% by mass or more, ZnO 1.0% by mass or more and 8.0% by mass or less, Al 2 O 3 15% by mass or more and 20% by mass or less, B2 O 3 and MgO in an amount of 2.0 mass % or more. 2 , ZnO, Al 2 O 3 , B 2 O 3 and MgO are components contained in glass fibers.

[0061] In particular, the glass cloth 3 is made of SiO 2 By including 59 mass % or more of the prepreg 1, the thermal expansion coefficient of the metal-clad laminate 10 formed from the prepreg 1 can be reduced.

[0062] Furthermore, when the glass cloth 3 contains 1.0 mass % or more and 8.0 mass % or less of ZnO, the thermal expansion coefficient of the metal-clad laminate 10 can be maintained low, while the hole position accuracy in drilling can be improved.

[0063] In addition, SiO 2 The content of B is preferably 75 mass % or less. 2 O 3 The content of MgO is preferably 9.0 mass % or less. The content of MgO is preferably 11.0 mass % or less.

[0064] The average thickness of the glass cloth 3 is preferably 40 μm or more, more preferably 50 μm or more, and even more preferably 60 μm or more. When the average thickness of the glass cloth 3 is 40 μm or more, the thermal expansion coefficient of the metal-clad laminate 10 can be easily reduced.

[0065] On the other hand, the average thickness of the glass cloth 3 is preferably 180 μm or less, more preferably 170 μm or less, and even more preferably 160 μm or less. When the average thickness of the glass cloth 3 is 180 μm or less, the metal-clad laminate 10 and the printed wiring board 100 can be made thinner. As a result, this contributes to making electronic devices lighter, thinner, shorter, and smaller.

[0066] The mass percentage of the glass cloth 3 relative to the total mass of the prepreg 1 is preferably 30 mass% or more, more preferably 40 mass% or more, and even more preferably 50 mass% or more. When the mass percentage of the glass cloth 3 is 30 mass% or more, it becomes easier to reduce the thermal expansion coefficient of the metal-clad laminate 10 while maintaining high hole position accuracy by drilling.

[0067] On the other hand, the mass percentage of the glass cloth 3 relative to the total mass of the prepreg 1 is preferably 70 mass% or less, more preferably 64 mass% or less, and even more preferably 60 mass% or less. When the mass percentage of the glass cloth 3 is 60 mass% or less, the thermal expansion coefficient of the metal-clad laminate 10 can be reduced while the hole position accuracy by drilling can be improved.

[0068] <Production Method> Depending on the type of thermosetting compound (A), etc., there are cases where the curing reaction of the thermosetting resin composition 2 can be stopped midway, and cases where the curing reaction of the thermosetting resin composition 2 proceeds all at once. Therefore, the production methods for the prepreg 1 will be explained below separately for the two cases.

[0069] When the curing reaction of the thermosetting resin composition 2 can be stopped midway, the thermosetting resin composition 2 is first liquefied using an appropriate solvent. Next, the liquid thermosetting resin composition 2 is impregnated into glass cloth 3. Next, the glass cloth 3 is heated to remove the solvent, and the curing reaction of the thermosetting resin composition 2 is advanced to an intermediate stage (i.e., B stage) and stopped there. This causes the thermosetting resin composition 2 to become semi-cured and is integrated with the glass cloth 3. As a result, a prepreg 1 is obtained.

[0070] On the other hand, if the curing reaction of the thermosetting resin composition 2 proceeds all at once, the liquid thermosetting resin composition 2 is impregnated into the glass cloth 3 in the same manner as described above. Next, the solvent is removed and the mixture is dried while being heated to a degree that does not cause the curing reaction of the thermosetting resin composition 2 to proceed. This allows the uncured thermosetting resin composition 2 to be integrated with the glass cloth 3. As a result, the prepreg 1 is obtained.

[0071] In this embodiment, in the thermosetting resin composition 2, the content of the inorganic filler (B) is 210 parts by mass or less per 100 parts by mass of the thermosetting compound (A), so that good moldability can be obtained when the thermosetting resin composition 2 is impregnated into the glass cloth 3.

[0072] 2, the metal-clad laminate 10 according to this embodiment is a substrate that extends in the X-axis direction and the Y-axis direction and has a thickness in the Z-axis direction. The metal-clad laminate 10 can be used as a material for a printed wiring board 100.

[0073] The metal-clad laminate 10 according to this embodiment includes an insulating layer including a cured product 4 of a prepreg 1 , and a metal layer 5 .

[0074] <Cured Product> The cured product 4 of the prepreg 1 is a cured product 4 of the thermosetting resin composition 2 integrated with the glass cloth 3. The cured product 4 refers to a C-stage substance. In this embodiment, the cured product 4 is in the form of a layer that extends in the X-axis direction and the Y-axis direction and has a thickness in the Z-axis direction. The cured product 4 has electrical insulation properties. In other words, the cured product 4 is included in the insulating layer. The cured product 4 may be the insulating layer itself.

[0075] <Metal Layer> The metal layer 5 is adhered to the cured product 4. The metal layer 5 is solid. The material of the metal layer 5 is not particularly limited, but examples thereof include copper. In this embodiment, the metal layer 5 includes a first metal layer 51 and a second metal layer 52. In this embodiment, the first metal layer 51 is adhered to a surface of the cured product 4 facing one side in the Z-axis direction. The second metal layer 52 is adhered to a surface of the cured product 4 facing the other side in the Z-axis direction.

[0076] <Manufacturing Method> A metal foil is laid on one or both sides of the prepreg 1, and the resulting mixture is heated and pressurized to obtain a metal-clad laminate 10. The heating and pressurization promotes a curing reaction of the thermosetting resin composition 2 integrated with the glass cloth 3 to form a cured product 4, and the metal foil is bonded to this cured product 4. The metal foil becomes a metal layer 5.

[0077] In this embodiment, the metal-clad laminate 10 is manufactured using the prepreg 1 described above, so that the coefficient of thermal expansion can be reduced and the accuracy of hole positioning by drilling can be improved.

[0078] 2 shows the metal-clad laminate 10 manufactured using one prepreg 1, the metal-clad laminate 10 may be manufactured by stacking two or more prepregs 1. In other words, two or more glass cloths 3 may be contained inside the cured material 4 contained in one insulating layer.

[0079] Furthermore, the metal-clad laminate 10 shown in Figure 2 is a double-sided metal-clad laminate because it includes both the first metal layer 51 and the second metal layer 52, but it may also be a single-sided metal-clad laminate that does not include either the first metal layer 51 or the second metal layer 52.

[0080] 3, the printed wiring board 100 according to this embodiment is a substrate that extends in the X-axis direction and the Y-axis direction and has a thickness in the Z-axis direction. The printed wiring board 100 can be used as a material for various electronic devices.

[0081] The printed wiring board 100 according to this embodiment includes an insulating layer including a cured product 4 of a prepreg 1 and conductor wiring 6 .

[0082] <Cured Product> The cured product 4 of the prepreg 1 is as described above.

[0083] <Conductor wiring> The conductor wiring 6 is adhered to the cured product 4. The conductor wiring 6 has an appropriate pattern shape when viewed from the Z-axis direction. The conductor wiring 6 is, for example, wiring used for transmitting signals and wiring used for supplying power. The material of the conductor wiring 6 is the same as the material of the metal layer 5. In this embodiment, the conductor wiring 6 includes a first conductor wiring 61 and a second conductor wiring 62. In this embodiment, the first conductor wiring 61 is adhered to a surface of the cured product 4 facing one side in the Z-axis direction. The second conductor wiring 62 is adhered to a surface of the cured product 4 facing the other side in the Z-axis direction.

[0084] <Manufacturing Method> The printed wiring board 100 is obtained by applying a subtractive process to the metal-clad laminate 10. That is, unnecessary portions of the metal layer 5 in the metal-clad laminate 10 are removed by etching to form conductor wiring 6 having a desired pattern shape. Although not shown in Fig. 3 , holes penetrating the printed wiring board 100 in the Z-axis direction may be drilled to connect the first conductor wiring 61 and the second conductor wiring 62 through the holes.

[0085] In this embodiment, the printed wiring board 100 is manufactured using the metal-clad laminate 10 described above, so that the coefficient of thermal expansion can be reduced and the accuracy of hole positioning by drilling can be improved.

[0086] 3 includes only two conductor wirings 6 (a first conductor wiring 61 and a second conductor wiring 62) sandwiched between the cured material 4 contained in the insulating layer, but may also be a multilayer printed wiring board including three or more conductor wirings 6. For example, a multilayer printed wiring board can be obtained by using the printed wiring board 100 shown in FIG. 3 as a core material and employing a build-up method.

[0087] 3. Aspects As is clear from the above embodiments, the present disclosure includes the following aspects. In the following, reference numerals are given in parentheses only to clarify the correspondence with the embodiments.

[0088] The first aspect is a prepreg (1) comprising a thermosetting resin composition (2) or a semi-cured product of the thermosetting resin composition (2), and glass cloth (3) integrated with the thermosetting resin composition (2) or the semi-cured product. The thermosetting resin composition (2) contains a thermosetting compound (A) and an inorganic filler (B). The content of the inorganic filler (B) is 90 parts by mass or more and 210 parts by mass or less per 100 parts by mass of the thermosetting compound (A). The glass cloth (3) contains SiO 2 59% by mass or more, ZnO 1.0% by mass or more and 8.0% by mass or less, Al 2 O 3 15% by mass or more and 20% by mass or less, B 2 O 3 and 2.0 mass % or more of MgO.

[0089] According to this aspect, it is possible to obtain good moldability while reducing the thermal expansion coefficient and improving the accuracy of hole positioning by drilling.

[0090] A second aspect is a prepreg (1) based on the first aspect, wherein the thermosetting compound (A) includes one or more compounds selected from the group consisting of epoxy resins, phenolic resins, cyanate resins, melamine resins, imide resins, and dicyandiamide.

[0091] According to this embodiment, it is possible to impart characteristics to the prepreg (1) according to various compounds.

[0092] A third aspect is the prepreg (1) based on the first or second aspect, wherein the inorganic filler (B) contains one or more particles selected from the group consisting of zinc molybdate particles, silica particles, aluminum hydroxide particles, talc particles, calcium molybdate particles, magnesium hydroxide particles, and boehmite particles.

[0093] According to this embodiment, it is possible to impart characteristics to the prepreg (1) according to the various particles.

[0094] A fourth aspect is the prepreg (1) based on any one of the first to third aspects. In the fourth aspect, the thermosetting resin composition (2) further contains a polymer (C) having a weight average molecular weight of 100,000 or more.

[0095] According to this embodiment, the coefficient of thermal expansion can be further reduced, and the thickness precision of the metal-clad laminate (10) can also be improved.

[0096] A fifth aspect is the prepreg (1) based on the fourth aspect. In the fifth aspect, the polymer (C) contains an acrylic monomer copolymer.

[0097] According to this embodiment, the coefficient of thermal expansion can be further reduced, and the thickness precision of the metal-clad laminate (10) can also be improved.

[0098] A sixth aspect is the prepreg (1) based on the fifth aspect. In the sixth aspect, the content of the acrylic monomer copolymer is 5 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the thermosetting compound (A).

[0099] According to this embodiment, the coefficient of thermal expansion can be further reduced, and the thickness precision of the metal-clad laminate (10) can also be improved.

[0100] A seventh aspect is the prepreg (1) based on any one of the first to sixth aspects. In the seventh aspect, the thermosetting resin composition (2) further contains core-shell rubber particles (D).

[0101] According to this aspect, the accuracy of hole positioning by drilling can be further improved.

[0102] An eighth aspect is the prepreg (1) based on the seventh aspect. In the eighth aspect, the mass ratio of the core-shell rubber particles (D) to the acrylic monomer copolymer is 3:2 to 8:2.

[0103] According to this embodiment, it becomes easier to obtain a synergistic effect of the acrylic monomer copolymer and the core-shell rubber particles (D) while maintaining high hole position accuracy by drilling.

[0104] A ninth aspect is a prepreg (1) based on any one of the first to eighth aspects. In the ninth aspect, the average thickness of the prepreg (1) is 45 μm or more and 200 μm or less.

[0105] According to this embodiment, the average thickness of the prepreg 1 is 45 μm or more, which makes it easier to reduce the thermal expansion coefficient of the metal-clad laminate 10. The average thickness of the prepreg 1 is 200 μm or less, which makes it possible to reduce the thickness of the metal-clad laminate 10 and the printed wiring board 100.

[0106] A tenth aspect is the prepreg (1) based on any one of the first to ninth aspects. In the tenth aspect, the mass percentage of the glass cloth (3) relative to the total mass of the prepreg (1) is 30 mass% or more.

[0107] According to this aspect, since the mass percentage of the glass cloth (3) is 30 mass% or more, it is easy to reduce the thermal expansion coefficient of the metal-clad laminate (10) while maintaining high hole position accuracy by drilling.

[0108] An eleventh aspect is a metal-clad laminate (10) comprising an insulating layer containing a cured product (4) of a prepreg (1) based on any one of the first to tenth aspects, and a metal layer (5).

[0109] According to this aspect, it is possible to obtain good moldability while reducing the thermal expansion coefficient and improving the accuracy of hole positioning by drilling.

[0110] A twelfth aspect is a printed wiring board (100) comprising an insulating layer containing a cured product (4) of a prepreg (1) based on any one of the first to tenth aspects, and conductor wiring (6).

[0111] According to this aspect, it is possible to obtain good moldability while reducing the thermal expansion coefficient and improving the accuracy of hole positioning by drilling.

[0112] The present disclosure will be specifically described below using examples, but the present disclosure is not limited to the following examples.

[0113] 1. Samples (1) Prepreg The raw materials used to manufacture the prepreg are listed below.

[0114] <Thermosetting Resin Composition> <Thermosetting Compound (A)> Epoxy resin (manufactured by Nippon Kayaku Co., Ltd., trade name "EPPN-502H", triphenylmethane type epoxy resin, epoxy equivalent: 158 to 178 g / eq) Phenol resin (manufactured by DIC Corporation, trade name "TD-2090", hydroxyl equivalent: 105 g / eq) <Inorganic Filler (B)> Silica particles (average particle diameter: 2.0 μm) Talc particles (average particle diameter: 3.3 μm) Zinc molybdate particles (average particle diameter: 3.3 μm) Aluminum hydroxide particles (average particle diameter: 4.6 μm) <Polymer (C)> Acrylic monomer copolymer (manufactured by Nagase ChemteX Corporation, trade name "SG-80H", weight average molecular weight: 350,000) <Core-shell Rubber Particles (D)> Core-shell rubber particles (manufactured by Mitsubishi Chemical Corporation, trade name "S-2200", average particle size: 0.1 μm) <Cure accelerator> 2-ethyl-4-methylimidazole <Glass cloth> The chemical composition of the glass cloth is shown in Table 1.

[0115] <Production of Prepreg> First, the above raw materials were blended in the composition shown in Table 1, and this blend was dissolved or dispersed in methyl ethyl ketone as a solvent, followed by stirring with a disperser, to prepare a liquid thermosetting resin composition.

[0116] Next, a glass cloth shown in Table 1 was impregnated with the above thermosetting resin composition, and heated at about 150°C for 4 to 5 minutes using a non-contact heating unit to dry and remove the solvent, thereby semi-curing the thermosetting resin composition to produce a prepreg.

[0117] (2) Metal-clad laminate Eight to sixteen sheets of the above prepreg are stacked, and these prepregs are sandwiched between two sheets of copper foil (thickness 12 μm) and subjected to a temperature of 220°C and a pressure of 2.94 MPa (30 kgf / cm 2 ) for 90 minutes to produce a copper clad laminate (CCL) having a thickness of about 1 mm.

[0118] 2. Evaluation (1) Hole Position Accuracy by Drilling Holes were drilled in a copper clad laminate (two layers) under the following drilling conditions:

[0119] Drill diameter: 0.15 mm (manufactured by Union Tool Co., Ltd.) Rotation speed: 250 krpm Feed speed: 3 m / min Entry board: 150 μm thick aluminum plate 10,000 holes were drilled, and the hole positions were measured using a hole tester (manufactured by Hitachi Via Mechanics Co., Ltd.). The average (Ave) (μm) and standard deviation (σ) (μm) of the deviation were then determined, and the value of "Ave + 3σ" (μm) was calculated based on these.

[0120] (2) Thermal expansion coefficient (α) A copper-clad laminate was immersed in an etching solution to remove the copper foil, yielding an insulating substrate (unclad substrate). The insulating substrate was dried at 80°C for 1 hour to remove moisture. The insulating substrate was cut into small pieces measuring 10 mm (Y-axis direction) x 3.5 mm (X-axis direction) x 1.0 mm (Z-axis direction), and the end faces were polished. The small pieces were baked at 230°C for 20 minutes to remove residual stress. The small pieces were then placed in a desiccator and cooled to room temperature.

[0121] The thermal expansion coefficient (α) of the small piece obtained as described above was measured under the following conditions.

[0122] Load: 10 mN Measurement start temperature: room temperature (but not more than 30°C) Heating rate: 10°C / min Measurement mode: compression method The thermal expansion coefficient (α) was calculated using the following formula.

[0123]

[0124] L: length of the small piece at 50°C (Y-axis direction) ΔL: difference between the length of the small piece at 260°C and the length of the small piece at 50°C ΔT: 210°C (= 260°C - 50°C) (3) Thickness Accuracy The thickness of the copper-clad laminate was measured at 80 points using a micrometer. The measurement points were spaced 55 mm apart. The standard deviation (σ) (μm) was calculated from the measurement results.

[0125] (4) Moldability The copper-clad laminate was immersed in an etching solution to remove the copper foil, thereby obtaining an insulating substrate (unclad substrate). Both sides of the insulating substrate were observed, and the presence or absence of smears (poor resin impregnation) was classified according to the following evaluation criteria to evaluate moldability.

[0126] S: No smears (poor resin impregnation) A: Smears (poor resin impregnation) occur only at the edges of the insulating substrate B: Smears (poor resin impregnation) occur not only at the edges but also in the center of the insulating substrate.

[0127]

[0128] As shown in Table 1, "Ave+3σ" in each example is 30 μm or less, which confirms that the hole position accuracy achieved by drilling is high.

[0129] Moreover, the thermal expansion coefficient of each example is 7 ppm / ° C. or less, which can be said to be sufficiently low.

[0130] Furthermore, the standard deviation of the plate thickness in each example is 8 μm or less, so it can be said that the plate thickness precision is high.

[0131] Furthermore, in each example, no smearing was observed, confirming that the moldability was also good.

[0132] REFERENCE SIGNS LIST 1 Prepreg 2 Thermosetting resin composition 3 Glass cloth 4 Cured product 5 Metal layer 6 Conductor wiring 10 Metal-clad laminate 100 Printed wiring board

Claims

1. A thermosetting resin composition or a semi-cured product of the thermosetting resin composition, and a glass cloth integrated with the thermosetting resin composition or the semi-cured product, wherein the thermosetting resin composition contains a thermosetting compound (A) and an inorganic filler (B), and the content of the inorganic filler (B) is 90 parts by mass or more and 210 parts by mass or less per 100 parts by mass of the thermosetting compound (A), and the glass cloth is made of SiO 2 59% by mass or more, ZnO is 1.0% by mass or more and 8.0% by mass or less, Al 2 O 3 15% by mass or more and 20% by mass or less, B 2 O 3 and 2.0 mass% or more of MgO.

2. The prepreg according to claim 1, wherein the thermosetting compound (A) comprises one or more compounds selected from the group consisting of epoxy resins, phenolic resins, cyanate resins, melamine resins, imide resins, and dicyandiamide.

3. The prepreg according to claim 1, wherein the inorganic filler (B) contains one or more types of particles selected from the group consisting of zinc molybdate particles, silica particles, aluminum hydroxide particles, talc particles, calcium molybdate particles, magnesium hydroxide particles, and boehmite particles.

4. The prepreg according to claim 1, wherein the thermosetting resin composition further contains a polymer (C) having a weight average molecular weight of 100,000 or more.

5. The prepreg according to claim 4, wherein the polymer (C) comprises an acrylic monomer copolymer.

6. The prepreg according to claim 5, wherein the content of the acrylic monomer copolymer is 5 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the thermosetting compound (A).

7. The prepreg according to claim 5, wherein the thermosetting resin composition further contains core-shell rubber particles (D).

8. The prepreg according to claim 7, wherein the mass ratio of the core-shell rubber particles (D) to the acrylic monomer copolymer is 3:2 to 8:

2.

9. The prepreg according to claim 1, wherein the average thickness of the prepreg is 45 μm or more and 200 μm or less.

10. The prepreg according to claim 1, wherein the mass percentage of the glass cloth relative to the total mass of the prepreg is 30 mass% or more.

11. A metal-clad laminate comprising an insulating layer containing a cured product of the prepreg according to any one of claims 1 to 10, and a metal layer.

12. A printed wiring board comprising an insulating layer containing a cured product of the prepreg according to any one of claims 1 to 10, and a conductor wiring.

Citation Information

Patent Citations

  • Resin composition, production method of resin composition, and prepreg and laminate each using the same

    JP2010260955A

  • Prepreg, metal-clad laminate and printed wiring board

    JP2018100327A

  • Glass compositions having low expansion and dielectric constants

    US4582748A

  • Glass fiber

    WO2012104999A1

  • Prepreg, metal-clad laminate board, and printed wiring board

    WO2017183621A1