(METH)acrylic acid copolymer, method for producing same, water treatment agent and scale inhibitor

A (meth)acrylic acid copolymer, with specific monomer units and molecular weight, addresses the opacity and foaming issues of conventional agents, effectively inhibiting scale formation and adhesion in industrial water systems, ensuring system efficiency and transparency.

WO2024203343A1PCT designated stage expired Publication Date: 2024-10-03TOAGOSEI(THAILAND) CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009811
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-13
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional water treatment agents used to prevent scale formation in piping systems are often opaque, prone to foaming, and ineffective in suppressing the formation of scales containing silica, calcium phosphate, and calcium sulfate, which can lead to efficiency issues and clogging in industrial water systems.

Method used

A (meth)acrylic acid-based copolymer is developed, comprising specific monomer units derived from (meth)acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid, and aromatic or vinyl monomers, with a controlled molecular weight and composition to create a transparent aqueous solution that effectively inhibits scale formation and adhesion without foaming, suitable for use in water treatment and scale adhesion prevention.

Benefits of technology

The copolymer solution is transparent, reduces foaming, and efficiently suppresses the formation of silica, calcium phosphate, and calcium sulfate scales, maintaining system efficiency and preventing adhesion in industrial water systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

A (meth)acrylic acid copolymer according to the present invention contains (a) a monomer unit derived from at least one substance selected from (meth)acrylic acid and salts thereof, (b) a monomer unit derived from at least one substance selected from 2-acrylamide-2-methylpropanesulfonic acid and salts thereof, and (c) a monomer unit derived from at least one monomer selected from aromatic vinyl monomers and vinyl monomers having a solubility of 7g or less in 100mL of water at 20°C or 30°C in the following proportions: 65.1-95.8 mass%, 4.1-34.8 mass%, and 0.1-4.9 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

(Meth)acrylic acid copolymer and method for producing the same, water treatment agent, and scale prevention agent

[0001] The present invention relates to a water treatment agent or a scale inhibitor that sufficiently inhibits the formation of scale containing at least silica among silica, calcium phosphate, calcium carbonate, and calcium sulfate, as well as a (meth)acrylic acid-based copolymer suitable as a main component thereof, and a method for producing the same.

[0002] Water has been used in various industries, and is usually transported through pipes. However, repeated transport or retention of water can cause scale formation on the inner surface of the pipes, including silicon compounds, calcium compounds, magnesium compounds, zinc compounds, etc., and therefore treatment agents (water treatment agents) are used to suppress such scale formation.

[0003] For example, Patent Document 1 discloses a method for preventing the spread of silica or silicate formation in an aqueous system, which comprises adding to the system: a) a water-soluble copolymer or terpolymer of (meth)acrylic acid or maleic acid or a salt thereof having a weight average molecular weight of about 1,000 to about 25,000, wherein the copolymer is composed of 1) about 20 to about 85% by weight of (meth)acrylic acid or maleic acid, and 2) greater than about 11 to about 80% by weight of (meth)acrylamidomethylpropanesulfonic acid or styrenesulfonic acid, or 3) about 5 to about 30% by weight of (meth)acrylamide or a substituted (meth)acrylamide, or 4) about 30 to about 60% by weight of isobutylene or diisobutylene; and the terpolymer is composed of 1) about 30 to about 80% by weight of (meth)acrylic acid or maleic acid, and 2) greater than about 11 to about 65% by weight of (meth)acrylamidomethylpropanesulfonic acid or styrenesulfonic acid. styrene sulfonic acid; and 3) about 5 to about 30% by weight of (meth)acrylamide or substituted (meth)acrylamide; or 4) about 5 to about 30% by weight of vinyl alcohol, allyl alcohol, esters of vinyl or allyl alcohol, vinyl esters, styrene, isobutylene, or diisobutylene; or 5) about 3 to about 30% by weight of styrene sulfonic acid when (meth)acrylaminomethylpropane sulfonic acid is present; b) magnesium ions; c) mixtures of said copolymers or terpolymers with aluminum ions or magnesium ions; and d) mixtures of poly(meth)acrylic acid or polymaleic acid or salts thereof having a weight average molecular weight of about 1,000 to about 25,000 with aluminum ions or magnesium ions.

[0004] Patent Document 2 discloses a method for stabilizing an aqueous system by inhibiting precipitation of inorganic salts, which comprises adding to the aqueous system: (a1) 40 to 60% by weight of an unsaturated sulfonic acid selected from one or more of 2-acrylamido-2-methyl-1-propanesulfonic acid, 2-methacrylamido-2-methyl-1-propanesulfonic acid, 3-methacrylamido-2-hydroxy-1-propanesulfonic acid, or salts thereof; and (b1) a water-soluble polymer having a weight average molecular weight of about 3,000 to about 10,000, which has monomer units of 40 to 60% by weight of an unsaturated carboxylic acid monomer selected from acrylic acid or methacrylic acid, or salts thereof; or (a2) one or more of 2-acrylamido-2-methyl-1-propanesulfonic acid, 2-methacrylamido-2-methyl-1-propanesulfonic acid, 3-methacrylamido-2-hydroxy-1-propanesulfonic acid, or salts thereof. (b2) 30 to 60% by weight of an unsaturated sulfonic acid selected from the above; (b3) 35 to 65% by weight of an unsaturated carboxylic monomer selected from acrylic acid or methacrylic acid or a salt thereof; and (c2) a water-soluble polymer having a weight average molecular weight of about 3,000 to about 12,000, the polymer having monomer units of 0.1 to 10% by weight of an unsaturated non-ionizable monomer selected from one or more of tert-butylacrylamide, tert-octylacrylamide, dimethylacrylamide, acrylamide, acryloylmorpholine, styrene, ethyl acrylate, butyl acrylate, hydroxyethyl methacrylate, or hydroxypropyl acrylate; the aqueous system contains inorganic ions selected from one or more of iron, zinc, calcium, phosphate, or molybdate ions; and maintaining the aqueous system at a temperature greater than about 80°C.

[0005] Patent Document 3 discloses an acrylic acid-based copolymer containing a structural unit (x) derived from acrylic acid or a sodium salt thereof and a structural unit (y) derived from 2-acrylamido-2-methylpropanesulfonic acid or a sodium salt thereof, the contents of the structural units (x) and (y) being 35 to 90% by mass and 10 to 65% by mass, respectively, when the total of the structural units is taken as 100% by mass, and the content of the acrylic acid-based copolymer having a weight-average molecular weight Mw of 2,000 to 30,000 and a molecular weight of 70,000 or more is 0.30% by mass or less relative to the total amount of all polymers. It also discloses that this acrylic acid-based copolymer is suitable as a component of a water treatment agent having the effect of inhibiting scale formation on calcium phosphate.

[0006] Patent Document 4 discloses a calcium phosphate and silica scale inhibitor as a treatment agent for effectively preventing the deposition of calcium phosphate and silica scale on heat exchangers and the like in open circulating cooling water systems, etc. The calcium phosphate and silica scale inhibitor is characterized in that the active ingredient is a copolymer of (meth)acrylic acid, (meth)acrylamidomethylpropanesulfonic acid, and a (meth)acrylamide derivative having an alkyl group having 1 to 8 carbon atoms, wherein, relative to 100% by weight of structural units derived from all monomers, the copolymer contains 40 to 70% by weight of structural units derived from (meth)acrylic acid, 15 to 40% by weight of structural units derived from (meth)acrylamidomethylpropanesulfonic acid, and 5 to 25% by weight of structural units derived from a (meth)acrylamide derivative having an alkyl group having 1 to 8 carbon atoms, and the copolymer contains a skeleton derived from a hypophosphorous acid compound in the polymer chain.

[0007] Japanese Patent Laid-Open No. 4-356580 Japanese Patent Laid-Open No. 8-224597 International Publication No. 2016 / 047267 Japanese Patent Laid-Open No. 2018-130702

[0008] Water treatment agents used to inhibit scale formation are usually aqueous solutions, and such water treatment agents are preferably transparent so that it is easy to visually determine whether they have acted on the water to be treated. Furthermore, since the scale formation inhibitory effect of the active ingredient, such as a polymer, is easily exerted, it is preferable that the agent is less likely to foam when mixed with water containing precursor components that form scale components, such as silica, calcium phosphate, calcium carbonate, or calcium sulfate. The object of the present invention is to provide a (meth)acrylic acid-based copolymer and a method for producing the same, which, when made into an aqueous solution, has excellent transparency, is less likely to foam when mixed with water (water to be treated) containing precursor components that form silica, calcium phosphate, calcium carbonate, calcium sulfate, etc., and satisfactorily inhibits the formation of scale containing at least silica from the group consisting of silica, calcium phosphate, calcium carbonate, and calcium sulfate, in the mixed solution.

[0009] The present inventors have discovered that when a (meth)acrylic acid-based copolymer containing these three monomer units in a specific ratio is dissolved in water, a transparent aqueous solution can be obtained; and when this aqueous solution is used as a water treatment agent and contacted with water (water to be treated) containing precursor components that form silica, calcium phosphate, calcium carbonate, or calcium sulfate, foaming is unlikely to occur, and the formation of scale containing these compounds is suppressed in each mixed solution of the water treatment agent and the water to be treated.

[0010] The present invention is illustrated below. [1] A (meth)acrylic acid-based copolymer comprising the following monomer units (a), (b), and (c): (a) monomer units derived from at least one monomer (ma) selected from the group consisting of (meth)acrylic acid and salts thereof; (b) monomer units derived from at least one monomer (mb) selected from the group consisting of 2-acrylamido-2-methylpropanesulfonic acid and salts thereof; and (c) monomer units derived from at least one monomer (mc) selected from the group consisting of vinyl monomers and aromatic vinyl monomers, the solubility of which in 100 mL of water at 20°C or 30°C is 7 g or less. When the total of the monomer units (a), (b), and (c) is taken as 100 mass%, the content of the monomer units (a), (b), and (c) in the (meth)acrylic acid-based copolymer is 65.1 to 95.8 mass%, 4.1 to 34.8 mass%, and 0.1 to 4.9 mass%, respectively. [2] The (meth)acrylic acid copolymer according to [1] above, wherein the monomer (mc) is at least one selected from styrene, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, and N-tert-butylacrylamide. [3] The (meth)acrylic acid copolymer according to [1] or [2] above, wherein the weight-average molecular weight is 1,500 to 20,000. [4] The (meth)acrylic acid copolymer according to any one of [1] to [3] above, wherein the content of the (meth)acrylic acid copolymer having a molecular weight of 1,000 or less is 15.0% by mass or less and the content of the (meth)acrylic acid copolymer having a molecular weight of 200,000 or more is 0.10% by mass or less, relative to the total amount of the (meth)acrylic acid copolymer. [5] A method for producing the (meth)acrylic acid-based copolymer according to any one of [1] to [4] above, comprising: a preparation step of preparing a monomer mixture containing the monomer (ma), the monomer (mb), the monomer (mc), and water, and a polymerization step of continuously supplying the monomer mixture, a polymerization initiator, and an optional chain transfer agent to a reactor and polymerizing the monomers. [6] A method for producing the (meth)acrylic acid-based copolymer according to [5] above, wherein in the polymerization step, the supply time of the monomer mixture to the reactor is 2 to 12 hours.[7] A method for producing a (meth)acrylic acid-based copolymer according to [5] or [6] above, wherein in the polymerization step, polymerization of the monomer is carried out while maintaining a total residual concentration of the monomer (mc) in the reactor of 0.3 g / 100 mL or less. [8] A water treatment agent containing the (meth)acrylic acid-based copolymer according to any one of [1] to [4] above. [9] An agent for preventing adhesion of calcium phosphate scale, calcium carbonate scale, calcium sulfate scale, and silica scale, containing the (meth)acrylic acid-based copolymer according to any one of [1] to [4] above.

[0011] In this specification, the weight average molecular weight (hereinafter also referred to as "Mw") and number average molecular weight (hereinafter also referred to as "Mn") of the polymer are values ​​calculated as standard sodium polyacrylate measured by gel permeation chromatography (hereinafter also referred to as "GPC"). In addition, the term "(meth)acrylic" means acrylic and methacrylic.

[0012] When the (meth)acrylic acid copolymer of the present invention is dissolved in water, a transparent aqueous solution can be obtained. When this aqueous solution is used as a water treatment agent and contacted with water (water to be treated) containing precursor components that form silica, calcium phosphate, calcium carbonate, or calcium sulfate, foaming is unlikely to occur, and the formation of scale containing at least silica among silica, calcium phosphate, calcium carbonate, and calcium sulfate can be suitably suppressed in a mixture of the water treatment agent and the water to be treated. Therefore, the (meth)acrylic acid copolymer of the present invention can also be used as a chemical component to prevent the adhesion of scale containing at least silica among silica, calcium phosphate, calcium carbonate, and calcium sulfate to the inner surface of a pipe or the like that comes into contact with water (water to be treated) containing precursor components that form scale. According to the method for producing a (meth)acrylic acid copolymer of the present invention, a (meth)acrylic acid copolymer having the above-mentioned effects can be efficiently produced.

[0013] The (meth)acrylic acid-based copolymer of the present invention (hereinafter referred to as "(meth)acrylic acid-based copolymer (P)") is characterized in that it comprises the following monomer units (a), (b), and (c), and when the total of these monomer units (a), (b), and (c) is taken as 100% by mass, the contents of the monomer units (a), (b), and (c) are 65.1 to 95.8% by mass, 4.1 to 34.8% by mass, and 0.1 to 4.9% by mass, respectively. (a) a monomer unit derived from at least one monomer (ma) selected from the group consisting of (meth)acrylic acid and salts thereof; (b) a monomer unit derived from at least one monomer (mb) selected from the group consisting of 2-acrylamido-2-methylpropanesulfonic acid and salts thereof; and (c) a monomer unit derived from at least one monomer (mc) selected from the group consisting of vinyl monomers and aromatic vinyl monomers having a solubility of 7 g or less in 100 mL of water at 20°C or 30°C.

[0014] The monomer unit (a) constituting the (meth)acrylic acid-based copolymer (P) of the present invention is derived from at least one kind of monomer (ma), and is a monomer unit derived from at least one selected from acrylic acid, an acrylic acid salt, methacrylic acid, and a methacrylic acid salt.

[0015] Examples of the monomer (ma) include acrylic acid, sodium acrylate, potassium acrylate, magnesium acrylate, calcium acrylate, methacrylic acid, sodium methacrylate, potassium methacrylate, magnesium methacrylate, and calcium methacrylate.

[0016] In the present invention, from the viewpoint of the transparency of an aqueous solution of the (meth)acrylic acid copolymer (P), the monomer units (a) preferably contain monomer units derived from an acrylate salt.

[0017] In the present invention, the content of the monomer unit (a) constituting the (meth)acrylic acid-based copolymer (P) is 65.1 to 95.8% by mass, where the total of the monomer units (a), (b), and (c) is 100% by mass. The lower limit is preferably 66.0% by mass, more preferably 67.0% by mass. The upper limit is preferably 80% by mass, more preferably 70% by mass.

[0018] The monomer unit (b) constituting the (meth)acrylic acid-based copolymer (P) of the present invention is derived from at least one kind of monomer (mb), and is a monomer unit derived from at least one selected from 2-acrylamido-2-methylpropanesulfonic acid and salts thereof.

[0019] Examples of the monomer (mb) include 2-acrylamido-2-methylpropanesulfonic acid and sodium 2-acrylamido-2-methylpropanesulfonate.

[0020] In the present invention, from the viewpoint of improving the solubility of the copolymer, the monomer unit (b) preferably contains a monomer unit derived from 2-acrylamido-2-methylpropanesulfonate.

[0021] In the present invention, the content of the monomer unit (b) constituting the (meth)acrylic acid-based copolymer (P) is 4.1 to 34.8% by mass, where the total of the monomer units (a), (b), and (c) is 100% by mass. The lower limit is preferably 10% by mass, more preferably 20% by mass. The upper limit is preferably 34.0% by mass, more preferably 33.0% by mass.

[0022] The monomer unit (c) constituting the (meth)acrylic acid-based copolymer (P) of the present invention is derived from at least one type of monomer (mc), and is at least one selected from the group consisting of vinyl monomers and aromatic vinyl monomers having a solubility of 7 g or less in 100 mL of water at 20°C or 30°C. Examples of vinyl monomers having a solubility of 7 g or less in 100 mL of water at 20°C or 30°C include ethyl acrylate, n-butyl acrylate, isobutyl acrylate, propyl vinyl ether, butyl vinyl ether, isobutyl vinyl ether, tert-butyl vinyl ether, butylene, isobutylene, and N-tert-butylacrylamide (TBAM). In the present invention, vinyl monomers having a solubility of 3 g or less are preferred, vinyl monomers having a solubility of 2 g or less are more preferred, vinyl monomers having a solubility of 1 g or less are even more preferred, and vinyl monomers having a solubility of 0.1 g or less are particularly preferred. Examples of aromatic vinyl monomers include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, β-methylstyrene, ethylstyrene, p-tert-butylstyrene, vinyltoluene, vinylxylene, and vinylnaphthalene.

[0023] In the present invention, from the viewpoints of the water solubility of the (meth)acrylic acid-based copolymer (P), the transparency of the resulting aqueous solution, and the ability to inhibit the formation of scale containing at least silica among silica, calcium phosphate, calcium carbonate, and calcium sulfate, the monomer units (c) preferably contain monomer units derived from ethyl acrylate, n-butyl acrylate, isobutyl acrylate, N-tert-butylacrylamide (TBAM), or styrene.

[0024] In the present invention, the content of the monomer unit (c) constituting the (meth)acrylic acid-based copolymer (P) is 0.1 to 4.9% by mass, where the total of the monomer units (a), (b), and (c) is 100% by mass. The lower limit is preferably 0.2% by mass, more preferably 0.4% by mass. The upper limit is preferably 3.0% by mass, more preferably 2.0% by mass.

[0025] Specific examples of the (meth)acrylic acid copolymer (P) of the present invention are shown below: (1) Acrylate / 2-acrylamido-2-methylpropanesulfonate / styrene copolymer (2) Acrylate / 2-acrylamido-2-methylpropanesulfonate / ethyl acrylate copolymer (3) Acrylate / 2-acrylamido-2-methylpropanesulfonate / n-butyl acrylate copolymer (4) Acrylate / 2-acrylamido-2-methylpropanesulfonate / isobutyl acrylate copolymer (5) Acrylate / 2-acrylamido-2-methylpropanesulfonate / N-tert-butylacrylamide (TBAM) copolymer

[0026] The structure of the (meth)acrylic acid copolymer (P) of the present invention is not particularly limited, but is preferably a random copolymer.

[0027] From the viewpoint of inhibiting the formation of scale containing at least silica among silica, calcium phosphate, calcium carbonate, and calcium sulfate, the Mw of the (meth)acrylic acid-based copolymer (P) of the present invention is preferably 1,500 to 20,000, more preferably 2,000 to 15,000, and even more preferably 3,000 to 10,000. The polydispersity, which is the ratio of Mw to Mn (Mw / Mn), is preferably 1.2 to 2.5, and more preferably 1.2 to 2.0.

[0028] The (meth)acrylic acid copolymer (P) of the present invention can be obtained by assembling copolymers of different molecular weights, and have the above-mentioned preferred Mw.Then, in the present invention, the (meth)acrylic acid copolymer (hereinafter referred to as "(meth)acrylic acid copolymer (P1)") with molecular weight of 1,000 or less or the (meth)acrylic acid copolymer (hereinafter referred to as "(meth)acrylic acid copolymer (P2)") with molecular weight of 200,000 or more may be included, but the content of (meth)acrylic acid copolymer (P1) is preferably 15.0% by mass or less, more preferably 10.0% by mass or less, even more preferably 5.0% by mass or less, and the content of (meth)acrylic acid copolymer (P2) is preferably 0.10% by mass or less, more preferably 0.05% by mass or less, based on the total amount of the (meth)acrylic acid copolymer (P) of the present invention.

[0029] The (meth)acrylic acid copolymer (P) of the present invention contains specific monomer units in specific content ratios and has the above-mentioned preferred Mw, thereby enabling the production of an aqueous solution with excellent transparency. When this aqueous solution is used as a water treatment agent and contacted with water (water to be treated) containing precursor components for forming silica, calcium phosphate, calcium carbonate, or calcium sulfate, foaming is suppressed, and the formation of scale containing at least silica among silica, calcium phosphate, calcium carbonate, and calcium sulfate can be suppressed in a mixture of the water treatment agent and the water to be treated. The inventors believe that the lack of foaming when the water treatment agent is mixed with the water to be treated is due to the fact that the monomer unit (c) has a hydrophobic group, and therefore, in the (meth)acrylic acid copolymer (P) containing 0.1 to 4.9 mass% of this monomer unit (c), the balance between the hydrophobic group and the hydrophilic group can be controlled within a range that does not act as a surfactant.

[0030] The (meth)acrylic acid copolymer (P) of the present invention can be produced by a conventionally known method. In order to obtain a preferable composition of the (meth)acrylic acid copolymer (P), not only the monomers may be polymerized but also the reaction product obtained by polymerization may be purified.

[0031] The method for producing a (meth)acrylic acid-based copolymer (P) according to the present invention (hereinafter referred to as the "production method of the present invention") sequentially comprises a preparation step of preparing a monomer mixture containing monomer (ma), monomer (mb), monomer (mc), and water, and a polymerization step of continuously supplying the resulting monomer mixture, a polymerization initiator, and an optional chain transfer agent to a reactor and polymerizing the monomers. When the monomers to be polymerized contain at least (meth)acrylic acid, i.e., (meth)acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid, and the (meth)acrylic acid-based copolymer (P) contains monomer units derived from a (meth)acrylate salt and / or monomer units derived from a 2-acrylamido-2-methylpropanesulfonate salt, it is preferable to subject the copolymer obtained by the polymerization step to a neutralization reaction (neutralization step) after the polymerization step. Furthermore, a step of removing unreacted monomers can be provided after either the polymerization step or the neutralization step.

[0032] In the above preparation step, the method for obtaining the monomer mixture is not particularly limited. In the present invention, since a hydrophobic monomer (mc) is used, it is preferable to first dissolve the monomer (mc) in the monomer (ma), and then mix the obtained solution with the monomer (mb) and water. The mixing method is not particularly limited.

[0033] The amounts of each monomer and water used in the above preparation step are as follows. The amount of monomer (ma) used is 65.1 to 95.8% by mass, based on the total amount of monomers (ma), (mb), and (mc). The lower limit is preferably 66.0% by mass, more preferably 67.0% by mass. The upper limit is preferably 80% by mass, more preferably 70% by mass. The amount of monomer (mb) used is 4.1 to 34.8% by mass, based on the total amount of monomers (ma), (mb), and (mc). The lower limit is preferably 10% by mass, more preferably 20% by mass. The upper limit is preferably 34.0% by mass, more preferably 33.0% by mass. The amount of monomer (mc) used is 0.1 to 4.9% by mass, based on the total amount of monomers (ma), (mb), and (mc). The lower limit is preferably 0.2% by mass, more preferably 0.4% by mass. The upper limit is preferably 3.0% by mass, more preferably 2.0% by mass. The amount of water used is preferably 5 to 80 parts by mass, more preferably 20 to 60 parts by mass, relative to 100 parts by mass of the total of the monomers (ma), (mb), and (mc).

[0034] Next, in the polymerization step, the monomer mixture obtained in the preparation step, a polymerization initiator, and an optional chain transfer agent are continuously supplied to a reactor, and the monomers are polymerized, preferably while stirring the reaction system. At this time, water may also be continuously supplied, if necessary. The reactor may be a conventional reactor (reaction apparatus) having a known configuration, equipped with a means for supplying a monomer mixture, a means for supplying a chain transfer agent, a means for supplying a polymerization initiator, a stirring means, a means for adjusting the temperature of the reaction system, a reflux cooling means, a means for supplying a neutralizing agent, a means for discharging the reaction liquid, and the like.

[0035] In the polymerization process according to the present invention, a copolymer having desired physical properties can be efficiently produced by setting the supply time of the monomer mixture to the reactor within a specific range. The supply time of the monomer mixture is preferably 2 to 12 hours, more preferably 2 to 10 hours, and even more preferably 2 to 6 hours. Note that the polymerization process is usually not completed simultaneously with the completion of the supply of the monomer mixture.

[0036] Furthermore, it is preferable that the feed rate of the monomer mixture to the reactor is constant, but the feed rate may be changed while checking the change in the polymerization conversion rate over time.

[0037] Examples of the polymerization initiator include hydrogen peroxide; persulfates such as sodium persulfate, potassium persulfate, and ammonium persulfate; dimethyl 2,2'-azobis(2-methylpropionate), 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), dimethyl 2,2'-azobis(isobutyrate), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methylpropionate), dimethyl 2,2'-azobis(isobutyrate), dimethyl 4,4'-azobis(4-cyanovaleric acid), dimethyl 2,2'-azobis(2-methylpropionate), dimethyl 2,2'-azobis(isobutyrate), dimethyl 4,4'-azobis(4-cyanovaleric acid), dimethyl 2,2'-azobis(2-methylpropionate), dimethyl 2,2'-azobis(2-methylpropionate), dimethyl 2,2'-azobis(isobutyronitrile ...2-methylpropionate), dimethyl 2,2'-azobis(2-methyl Examples of the suitable azo compounds include 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] dihydrochloride, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] n-hydrate, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] disulfate dihydrate, and 1,1'-azobis(cyclohexane-1-carbonitrile); and organic peroxides such as benzoyl peroxide, lauroyl peroxide, peracetic acid, di-t-butyl peroxide, and cumene hydroperoxide. These may be used alone or in combination of two or more.

[0038] The amount of the polymerization initiator used is preferably 0.1 to 10.0 parts by mass, more preferably 0.1 to 2.0 parts by mass, per 100 parts by mass of the total of the monomers (ma), (mb) and (mc).

[0039] The method of using the polymerization initiator is not particularly limited, and it is preferable to start the supply of the polymerization initiator simultaneously with the supply of the monomer mixture, or to start the supply of the polymerization initiator after the supply of the monomer mixture. The supply of the polymerization initiator is completed preferably 5 minutes or more, particularly preferably 10 minutes or more, later than the completion of the supply of the monomer mixture.

[0040] Examples of chain transfer agents include phosphorous acid, hypophosphorous acid, and salts thereof (sodium hypophosphite, potassium hypophosphite, etc.); sulfurous acid, hydrogen sulfite, dithionous acid, metabisulfite, and salts thereof (sodium hydrogen sulfite, potassium hydrogen sulfite, sodium dithionite, potassium dithionite, sodium metabisulfite, potassium metabisulfite, etc.); and thiols such as mercaptoethanol, thioglycerol, thioglycolic acid, 2-mercaptopropionic acid, 3-mercaptopropionic acid, thiomalic acid, octyl thioglycolate, octyl 3-mercaptopropionate, 2-mercaptoethanesulfonic acid, n-dodecyl mercaptan, octyl mercaptan, and butyl thioglycolate. These may be used alone or in combination of two or more.

[0041] The amount of the chain transfer agent used is preferably 0.1 to 30 parts by mass, more preferably 1 to 15 parts by mass, per 100 parts by mass of the total of the monomers (ma), (mb) and (mc).

[0042] The method for using the chain transfer agent is not particularly limited, and the supply thereof is completed preferably 10 minutes or more, particularly preferably 20 minutes or more, earlier than the completion time of the supply of the monomer mixture.

[0043] In the polymerization step, the presence of polyvalent metal ions in the reaction system can promote the decomposition of the polymerization initiator and the chain transfer agent during the polymerization reaction. Materials that form such polyvalent metal ions include ammonium iron(III) sulfate or its hydrate, iron(III) sulfate or its hydrate, and iron(II) sulfate or its hydrate.

[0044] In the polymerization step, it is preferable to add water to the reactor before supplying each raw material to the reactor, so that the raw materials supplied to the reactor are mixed efficiently and the polymerization reaction proceeds smoothly. The added material can be water alone, water containing a chain transfer agent, or water containing polyvalent metal ions.

[0045] The polymerization temperature of the monomers in the polymerization step (temperature of the reaction system) is appropriately selected depending on the type of polymerization initiator, etc., and is not particularly limited. A preferred polymerization temperature is 70°C or higher. In a reaction system in which no side reactions occur, the temperature is preferably near the boiling point of the polymerization solvent (water), and particularly preferably the boiling point of the polymerization solvent (water). When the supply of the polymerization initiator is started after the start of the supply of the monomer mixture, the temperature of the reaction system at the start of the supply of the monomer mixture may be lower than the predetermined polymerization temperature. In this case, the temperature can be adjusted to the predetermined polymerization temperature after the start of the supply of the polymerization initiator.

[0046] In the polymerization step according to the present invention, the residual concentration (total concentration) of the monomer (mc) per 100 mL of reaction solution in the reactor can be adjusted to preferably 0.3 g or less, more preferably 0.1 g or less, throughout the entire process from the start of polymerization to the completion of the supply of the polymerization initiator, thereby enabling efficient production of a (meth)acrylic acid-based copolymer (P) having desired physical properties. The polymerization step is preferably completed after a maximum of 13 hours have elapsed since the completion of the supply of the monomer mixture.

[0047] When the production method of the present invention includes a neutralization step after the polymerization step, an alkaline agent or an aqueous solution thereof can be used, such as an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide; an alkaline earth metal hydroxide such as calcium hydroxide or magnesium hydroxide; ammonia; an organic amine salt such as monoethanolamine or triethanolamine. As the alkaline agent, an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide is preferred, and sodium hydroxide is particularly preferred.

[0048] When the neutralization step is carried out, the pH of the reaction solution is adjusted to preferably 7.0 or less, more preferably in the range of 1.0 to 5.0.

[0049] According to the production method of the present invention, it is possible to efficiently produce a (meth)acrylic acid-based copolymer (P) in which the content ratios of the monomer units (a), (b), and (c) are within a predetermined range, and the content of the unreacted monomers (ma), (mb), and (mc) and the content of the above-mentioned (meth)acrylic acid-based copolymers (P1) and (P2) are all as small as possible.

[0050] When water is not removed from the reaction solution after the polymerization step and the neutralization step in the production method of the present invention, the reaction solution usually consists of an aqueous solution of the (meth)acrylic acid copolymer (P). Using this aqueous solution, it is possible to easily produce water treatment agents that suppress scale formation in cooling water systems, boiler water systems, geothermal power generation water systems, seawater desalination plants, pulp dissolving pots, black liquor concentrating pots, etc., and scale inhibitors that prevent scale deposition on the inner surfaces of cooling water pipes and heat transfer surfaces of heat exchangers, etc. Furthermore, since the aqueous solution of the (meth)acrylic acid copolymer (P) can be made clear and transparent, the water treatment agents and scale inhibitors obtained using this aqueous solution can also be transparent and easy to handle.

[0051] The water treatment agent of the present invention contains a (meth)acrylic acid-based copolymer (P) and is preferably in the form of a liquid (aqueous solution). The content of the (meth)acrylic acid-based copolymer (P) in this aqueous solution is preferably 1 to 1000 mg / L, more preferably 5 to 100 mg / L, since the effect as a water treatment agent, i.e., the effect of inhibiting scale formation, can be sufficiently obtained.

[0052] The water treatment agent of the present invention may contain, as necessary, conventionally known scale formation inhibitors, bactericides, anticorrosives, slime inhibitors, defoamers, etc., such as polyacrylic acid or a salt thereof, polymaleic acid or a salt thereof, other (meth)acrylic acid copolymers, and styrene-maleic acid copolymers.

[0053] The water treatment agent of the present invention is suitable for application to water (water to be treated) containing precursor components that form at least silica scale, selected from silica scale, calcium phosphate scale, calcium carbonate scale, and calcium sulfate scale. For example, in open-circulation cooling water systems, in order to reduce the amount of cooling water discharged outside the system from the perspective of water and resource conservation, the cooling water may be concentrated, forming poorly soluble salts such as calcium phosphate and calcium carbonate. In such cases, use of the water treatment agent of the present invention can suppress problems such as reduced heat exchange efficiency and pipe blockage. Furthermore, silica scale may form in cooling water systems, boiler water systems, or geothermal power generation water systems that are equipped with heat exchangers, refrigerators, etc. and operate at high concentrations. Once silica scale adheres to the components of the equipment, its removal is often difficult. Therefore, use of the water treatment agent of the present invention can effectively suppress the formation of silica scale. The pH and temperature of the water (water to be treated) are not particularly limited.

[0054] When the water treatment agent of the present invention is used, for example, it is added to water (water to be treated) containing the precursor components that form the scale material, and stirred as necessary.

[0055] The scale preventive agent of the present invention contains a (meth)acrylic acid copolymer (P) and is preferably in the form of a liquid (aqueous solution). The content of the (meth)acrylic acid copolymer (P) in this aqueous solution is preferably 1 to 1000 mg / L, more preferably 5 to 100 mg / L, since the effect as a scale preventive agent, for example, the effect of preventing scale buildup on structural members such as condensers, heat exchangers, and piping that come into contact with water such as industrial water, tap water, and groundwater, can be sufficiently obtained.

[0056] When the scale preventive agent of the present invention is used, it is added to water (water to be treated) containing the precursor components that form the above-mentioned scale materials, and stirred as necessary.

[0057] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to these examples. In the following, % and ppm are by mass unless otherwise specified.

[0058] 1. Raw materials for producing (meth)acrylic acid copolymers Various polymers were produced using the following raw materials.

[0059] 1-1. Monomers AA: Acrylic acid ATBS: Sodium 2-acrylamido-2-methylpropanesulfonate St: Styrene EA: Ethyl acrylate The solubility in 100 mL of water at 20°C is 1.5 g. BA: n-butyl acrylate The solubility in 100 mL of water at 20°C is 0.14 g. IBA: Isobutyl acrylate The solubility in 100 mL of water at 20°C is 0.79 g. TBAM: N-tert-butylacrylamide The solubility in 100 mL of water at 30°C is 0.1 g.

[0060] 1-2. Polymerization initiator: sodium persulfate

[0061] 1-3. Chain transfer agent: sodium bicarbonate

[0062] 1-4. Neutralizer: 50% aqueous solution of sodium hydroxide

[0063] 2. Evaluation method for (meth)acrylic acid copolymer or its aqueous solution 2-1. Measurement of molecular weight distribution of (meth)acrylic acid copolymer The Mw and Mn of the (meth)acrylic acid copolymer were measured by GPC using an "LC-20AD" (model name) manufactured by Shimadzu Corporation. <GPC measurement conditions> Column: G4000PWxl, G3000PWxl, and G2500PWxl manufactured by Tosoh Corporation connected together Eluent: 0.1M NaCl + phosphate buffer (pH 7) Detector: RI Column temperature: 40°C Standard material: sodium polyacrylate manufactured by Sowa Scientific Co., Ltd.

[0064] 2-2. Quantitative Determination of Unreacted Monomers in (Meth)acrylic Acid Copolymers (1) AA or its sodium salt and ATBS were measured by high performance liquid chromatography (hereinafter referred to as "HPLC") using an "LC-20AD" (model name) manufactured by Shimadzu Corporation. <HPLC Measurement Conditions> Column: ODS-80Ts manufactured by Tosoh Corporation Eluent: 0.17% aqueous tetrabutylammonium hydrogen sulfide solution: acetonitrile = 90:10 Column temperature: 40°C Detector: UV-vis (205 nm)

[0065] 2-3. Quantitative Determination of Unreacted Monomers in (Meth)acrylic Acid-Based Copolymer (2) St, EA, BA, IBA, and TBAM were measured by gas chromatography (hereinafter referred to as "GC") using a Shimadzu "GC-2014AF" (model name). <GC Measurement Conditions> Column: Tosoh HR-1 Carrier Gas: He Sample Inlet Temperature: 250°C Heating Conditions: 70°C → 150°C (Heating Rate: 20°C per Minute) Detector: FID Detector Temperature: 250°C

[0066] 3. Production of (meth)acrylic acid copolymers Production examples of various (meth)acrylic acid copolymers are shown below.

[0067] Example 1-1 First, 1.4 g of styrene (St) was dissolved in 475 g of acrylic acid (AA). To this mixture, 496 g of a 50% aqueous solution of sodium 2-acrylamido-2-methylpropanesulfonate (ATBS) and 14 g of pure water were added and thoroughly stirred to obtain a monomer mixture. Subsequently, 420 g of pure water was charged into a reactor equipped with a reflux condenser, and the temperature was raised to 75°C. Then, 9 g of a 30% aqueous solution of sodium bisulfite was added while stirring the contents of the reactor. The above monomer mixture, a 5% aqueous solution of sodium persulfate, and a 30% aqueous solution of sodium bisulfite were continuously fed into the reactor to carry out a polymerization reaction. The feed rate and feed time of the monomer mixture were 4.1 g / min and 4 hours, respectively. The feed rate and feed time of the 5% aqueous solution of sodium persulfate were 0.3 g / min and 4 hours and 10 minutes, respectively. The supply rate and supply time of the 30% aqueous solution of sodium bisulfite were 0.7 g / min and 3 hours and 40 minutes, respectively. During the polymerization reaction, the temperature inside the reactor was maintained at 75°C. Furthermore, the residual concentration of styrene (St), the monomer (mc), per 100 mL of reaction solution was maintained at less than 0.1 g. After the supply of the 5% aqueous solution of sodium persulfate was completed, the reaction solution was heated to 85°C and maintained at this temperature for 1 hour. Next, the pH of the reaction solution was adjusted to 2.3 using a neutralizing agent, and an aqueous solution of a (meth)acrylic acid-based copolymer (hereinafter also referred to as "copolymer (E1)") with a solids concentration of 42% was obtained. This aqueous solution was clear and transparent.

[0068] A sample taken one hour after the start of polymerization was subjected to gas chromatography (GC), and the residual concentration of the monomer (mc) was found to be less than 0.1 g / 100 mL (see Table 1).

[0069] Thereafter, copolymer (E1) was subjected to gel permeation chromatography (GPC), which revealed that the copolymer had an Mw of 9570, an Mn of 4830, and an Mw / Mn ratio of about 2.0. The content of (meth)acrylic acid-based copolymers having a molecular weight of 1000 or less in copolymer (E1) was 0.6%, and the content of (meth)acrylic acid-based copolymers having a molecular weight of 200000 or more was 0.0% (see Table 1).

[0070] Furthermore, quantitative analysis of the unreacted monomers contained in the copolymer (E1) revealed that AA and its sodium salt were 55 ppm, ATBS was 125 ppm, and St was below the detection limit (1 ppm) (see Table 1).

[0071] Examples 1-2 to 1-9 Using monomers having the compositions shown in Table 1, (meth)acrylic acid copolymers (E2) to (E9) were produced in the same manner as in Example 1-1 (see Table 1).

[0072] Comparative Example 1-1 First, 473 g of acrylic acid (AA), 496 g of a 50% aqueous solution of sodium 2-acrylamido-2-methylpropanesulfonate (ATBS), and 14 g of pure water were thoroughly stirred to obtain a monomer mixture. Subsequently, 420 g of pure water was charged into a reactor equipped with a reflux condenser, and the temperature was raised to 75°C. Then, 9 g of a 30% aqueous solution of sodium bisulfite was added while stirring the contents of the reactor. The above monomer mixture, a 5% aqueous solution of sodium persulfate, and a 30% aqueous solution of sodium bisulfite were continuously fed into the reactor to carry out a polymerization reaction. The feed rate and feed time of the monomer mixture were 4.1 g / min and 4 hours, respectively. The feed rate and feed time of the 5% aqueous solution of sodium persulfate were 0.3 g / min and 4 hours 10 minutes, respectively. The feed rate and feed time of the 30% aqueous solution of sodium bisulfite were 0.7 g / min and 3 hours 40 minutes, respectively. During the polymerization reaction, the temperature inside the reactor was maintained at 75°C. After the supply of the 5% aqueous solution of sodium persulfate was completed, the reaction solution was heated to 85°C and maintained at this temperature for 1 hour. Next, the pH of the reaction solution was adjusted to 2.3 using a neutralizing agent to obtain an aqueous solution of a (meth)acrylic acid-based copolymer (hereinafter also referred to as "copolymer (EE1)") with a solids concentration of 45%. This aqueous solution was clear and transparent.

[0073] Thereafter, copolymer (EE1) was subjected to gel permeation chromatography (GPC), which revealed that the copolymer had an Mw of 6730, an Mn of 4130, and an Mw / Mn ratio of approximately 1.6. The content of (meth)acrylic acid-based copolymers having a molecular weight of 1000 or less in copolymer (EE1) was 0.8%, and the content of (meth)acrylic acid-based copolymers having a molecular weight of 200000 or more was 0.0% (see Table 1).

[0074] Furthermore, quantitative analysis of the unreacted monomers contained in the copolymer (EE1) revealed that the amounts of AA and its sodium salt were 66 ppm, and ATBS was 123 ppm (see Table 1).

[0075] Comparative Example 1-2: First, 35 g of styrene (St) was dissolved in 315 g of acrylic acid (AA). To this mixture, 774 g of a 50% aqueous solution of sodium 2-acrylamido-2-methylpropanesulfonate (ATBS) and 14 g of pure water were added and thoroughly stirred to obtain a monomer mixture. Subsequently, 420 g of pure water was charged into a reactor equipped with a reflux condenser, and the temperature was raised to 75°C. Then, 9 g of a 30% aqueous solution of sodium bisulfite was added while stirring the contents of the reactor. The above monomer mixture, a 5% aqueous solution of sodium persulfate, and a 30% aqueous solution of sodium bisulfite were continuously fed into the reactor to carry out a polymerization reaction. The feed rate and feed time of the monomer mixture were 4.7 g / min and 4 hours, respectively. The feed rate and feed time of the 5% aqueous solution of sodium persulfate were 0.3 g / min and 4 hours and 10 minutes, respectively. The supply rate and supply time of the 30% aqueous solution of sodium bisulfite were 0.7 g / min and 3 hours and 40 minutes, respectively. The temperature inside the reactor was maintained at 75°C during the polymerization reaction. After the supply of the 5% aqueous solution of sodium persulfate was completed, the reaction solution was heated to 85°C and maintained at this temperature for 1 hour. The pH of the reaction solution was then adjusted to 2.6 using a neutralizing agent, yielding an aqueous solution of a (meth)acrylic acid-based copolymer (hereinafter referred to as "copolymer (EE2)") with a solids concentration of 42%. This aqueous solution was turbid and opaque.

[0076] A sample taken one hour after the start of polymerization was subjected to gas chromatography (GC), and the residual concentration of the monomer (mc) was found to be less than 0.1 g / 100 mL (see Table 1).

[0077] Thereafter, copolymer (EE2) was subjected to gel permeation chromatography (GPC), which revealed that the copolymer had an Mw of 7700, an Mn of 4640, and an Mw / Mn ratio of approximately 1.7. The content of (meth)acrylic acid-based copolymers having a molecular weight of 1000 or less in copolymer (EE2) was 0.5%, and the content of (meth)acrylic acid-based copolymers having a molecular weight of 200000 or more was 0.0% (see Table 1).

[0078] Furthermore, quantitative analysis of the unreacted monomers contained in the copolymer (EE2) revealed that the amounts of AA and its sodium salt were 66 ppm, and ATBS was 628 ppm (see Table 1).

[0079] Comparative Example 1-3 First, 70 g of styrene (St) was dissolved in 469 g of acrylic acid (AA), and to this mixture were added 357 g of a 50% aqueous solution of sodium 2-acrylamido-2-methylpropanesulfonate (ATBS) and 14 g of pure water, followed by thorough stirring to obtain a monomer mixture. Subsequently, 420 g of pure water was charged into a reactor equipped with a reflux condenser, and the temperature was raised to 75°C. Then, 9 g of a 30% aqueous solution of sodium bisulfite was added while stirring the contents of the reactor. Then, while maintaining the temperature inside the reactor at 75°C, the polymerization reaction was initiated by changing the feed rate and feed time of the monomer mixture into the reactor to 3.8 g / min and 4 hours, respectively, the feed rate and feed time of the 5% aqueous solution of sodium persulfate to 0.3 g / min and 4 hours 10 minutes, respectively, and the feed rate and feed time of the 30% aqueous solution of sodium bisulfite to 0.7 g / min and 3 hours 40 minutes, respectively. However, during the polymerization reaction, precipitates were formed inside the reactor, and production of the (meth)acrylic acid-based copolymer (hereinafter referred to as "copolymer (EE3)") was discontinued.

[0080]

[0081] 4. Evaluation of Water Treatment Agents (1) Scale Inhibition Test for Silica, Calcium Phosphate, Calcium Carbonate, and Calcium Sulfate Each aqueous solution of the (meth)acrylic acid copolymer obtained in Examples 1-1 to 1-9 and Comparative Examples 1-1 to 1-2 above was adjusted to a (meth)acrylic acid copolymer concentration of 1000 ppm to prepare a water treatment agent (S), and its effect of inhibiting scale formation for silica, calcium phosphate, calcium carbonate, and calcium sulfate was confirmed by the following method. The results are shown in Table 2. In the calcium phosphate scale inhibition test, calcium carbonate scale inhibition test, and calcium sulfate scale inhibition test below, "blank" refers to the test results of a solution in which the inorganic salt was adjusted to a predetermined concentration without adding the water treatment agent (S).

[0082] <Silica Scale Inhibition Test> Using the water treatment agent (S) and sodium silicate, 240 mL of a solution containing a (meth)acrylic acid copolymer at a concentration of 150 mg / L and a sodium silicate at a concentration of 351 mg / L was prepared and left at 70 ° C. for 30 minutes. Then, while stirring this solution, 44 mL of a 0.5% magnesium chloride aqueous solution, 31.6 mL of a 0.5% calcium chloride aqueous solution, and 36 mL of a 0.5% sodium bicarbonate aqueous solution were added. Next, while stirring this mixed solution, 40 mL of a 0.21% sodium bicarbonate aqueous solution was added, and the pH was adjusted to 8.0 with a 1 mol / L hydrochloric acid aqueous solution. After that, after leaving it at 70 ° C. for 3 hours, the liquid was visually observed for turbidity and precipitation due to silica, and the scale inhibition ability was evaluated according to the following criteria. ⊚: No precipitation was observed, but the liquid was slightly turbid. ◯: No precipitation was observed, but the liquid was heavily turbid. ×: Precipitation was observed.

[0083] <Calcium Phosphate Scale Inhibition Test> Using the water treatment agent (S), disodium hydrogen phosphate, and calcium chloride, 360 mL of a solution containing a (meth)acrylic acid copolymer concentration of 20 mg / L, a disodium hydrogen phosphate concentration of 90 mg / L, and a calcium chloride concentration of 375 mg / L was prepared. Next, while stirring this solution, 40 mL of a 0.21% aqueous sodium bicarbonate solution was added, and the pH was adjusted to 8.5 with a 0.1 mol / L aqueous sodium hydroxide solution. After leaving it at 60°C for 3 hours, the solution was visually observed for turbidity and precipitation due to calcium phosphate, and the scale inhibition ability was evaluated according to the following criteria: ◎: No turbidity or precipitation was observed; ○: Turbidity and precipitation were observed, but the Ca concentration in the supernatant after filtration was higher than in the blank; ×: Turbidity and precipitation were observed, but there was no difference in the Ca concentration in the supernatant after filtration compared to the blank.

[0084] <Calcium Carbonate Scale Inhibition Test> Using the water treatment agent (S), sodium bicarbonate, and calcium chloride, 400 mL of a solution containing a (meth)acrylic acid copolymer concentration of 10 mg / L, a sodium bicarbonate concentration of 420 mg / L, and a calcium chloride concentration of 375 mg / L was prepared. The pH of this solution was then adjusted to 8.5 with a 1 M aqueous sodium hydroxide solution. After leaving the solution at 60°C for 20 hours, the solution was visually observed for turbidity and precipitation due to calcium carbonate, and the scale inhibition was evaluated according to the following criteria: ◎: No turbidity or precipitation was observed; ○: Turbidity and precipitation were observed, but the Ca concentration in the supernatant after filtration was higher than in the blank; ×: Turbidity and precipitation were observed, but there was no difference in the Ca concentration in the supernatant after filtration compared to the blank.

[0085] <Calcium sulfate scale inhibition test> Using the water treatment agent (S), sodium sulfate, and calcium chloride, 400 mL of a solution was prepared, the solution having a (meth)acrylic acid copolymer concentration of 4 mg / L, a sodium sulfate concentration of 6000 mg / L, and a calcium chloride concentration of 6200 mg / L. After leaving the solution at 60°C for 3 hours, the solution was visually observed for turbidity and precipitation due to calcium sulfate, and the scale inhibition ability was evaluated according to the following criteria: ◎: No turbidity or precipitation was observed; ○: Turbidity and precipitation were observed, but the Ca concentration in the supernatant after filtration was higher compared to the blank; ×: Turbidity and precipitation were observed, but there was no difference in the Ca concentration in the supernatant after filtration compared to the blank.

[0086] (2) Foaming Evaluation Test Each aqueous solution of the (meth)acrylic acid copolymer obtained in Examples 1-1 to 1-9 and Comparative Examples 1-1 to 1-2 above was adjusted to a concentration of 1% (meth)acrylic acid copolymer to prepare a water treatment agent (T), and 10 g of the solution was placed in a resin disposable cup manufactured by AS ONE (volume: 1 L, size: upper diameter 122 mm, lower diameter 102.5 mm, height 147 mm) and stirred at maximum speed for 30 seconds using a SCARLETT hand mixer "SUPER HAND MIXER MODEL HE-133" (attachment is beater type). The foaming height immediately after the start of stirring and the time from the start of stirring until the generated foam disappeared were measured, and the foaming property was evaluated according to the following criteria. The results are shown in Table 2. ◎: Almost no foaming occurred immediately after stirring (approximately 1 cm or less), and the foam disappeared immediately (approximately within 15 seconds). ○: The foam disappeared within approximately 1 minute after stirring. ×: The foam did not disappear within approximately 1 minute after stirring.

[0087]

[0088] Examples 2-1 to 2-4 are examples using (meth)acrylic acid copolymers E1 to E4 containing 70% or less of the monomer unit (a), and showed particularly excellent performance in all of the following: silica deposition inhibition, calcium phosphate formation inhibition, calcium carbonate formation inhibition, and calcium sulfate formation inhibition. Examples 2-1 to 2-3 are examples using (meth)acrylic acid copolymers E1 to E3 containing 2.0% or less of the monomer unit (c), and showed excellent results in foaming evaluation, with foaming immediately after stirring being suppressed.

[0089] Examples 2-5 to 2-9 are examples using (meth)acrylic acid copolymers E5 to E9, which showed a certain effect in inhibiting silica deposition and excellent performance in inhibiting calcium phosphate formation, calcium carbonate formation, and calcium sulfate formation. Furthermore, Examples 2-5 to 2-7 showed excellent results in the foaming evaluation, with foaming immediately after stirring being suppressed.

[0090] On the other hand, no silica deposition inhibitory effect was obtained in Comparative Examples 2-1 and 2-2. The (meth)acrylic acid-based copolymers EE2 and EE3 of Comparative Examples 2-2 and 2-3 are not sufficiently water-soluble and cannot be used as a water treatment agent or a constituent component of a scale inhibitor having an effect of inhibiting scale deposition on components of equipment in a cooling water system, a boiler water system, or a geothermal power generation water system.

[0091] The (meth)acrylic acid-based copolymer of the present invention is suitable as a constituent component of a water treatment agent containing at least silica among silica, calcium phosphate, calcium carbonate, and calcium sulfate, which has an excellent effect of inhibiting scale formation, or a scale inhibitor having an excellent effect of inhibiting scale deposition on components of equipment in cooling water systems, boiler water systems, or geothermal power generation water systems.

Claims

1. A (meth)acrylic acid-based copolymer comprising the following monomer units (a), (b) and (c): (a) a monomer unit derived from at least one monomer (ma) selected from the group consisting of (meth)acrylic acid and its salts; (b) a monomer unit derived from at least one monomer (mb) selected from the group consisting of 2-acrylamido-2-methylpropanesulfonic acid and its salts; and (c) a monomer unit derived from at least one monomer (mc) selected from the group consisting of vinyl monomers and aromatic vinyl monomers having a solubility of 7 g or less in 100 mL of water at 20°C or 30°C. When the total of the monomer units (a), (b) and (c) is taken as 100 mass%, the content ratios of the monomer units (a), (b) and (c) are 65.1 to 95.8 mass%, 4.1 to 34.8 mass% and 0.1 to 4.9 mass%, respectively.

2. The (meth)acrylic acid-based copolymer according to claim 1, wherein the monomer (mc) is at least one selected from the group consisting of styrene, ethyl acrylate, n-butyl acrylate, isobutyl acrylate and N-tert-butylacrylamide.

3. The (meth)acrylic acid copolymer according to claim 1 or 2, which has a weight average molecular weight of 1,500 to 20,000.

4. The (meth)acrylic acid-based copolymer according to any one of claims 1 to 3, wherein the content of the (meth)acrylic acid-based copolymer having a molecular weight of 1,000 or less is 15.0 mass% or less, and the content of the (meth)acrylic acid-based copolymer having a molecular weight of 200,000 or more is 0.10 mass% or less, based on the total amount of the (meth)acrylic acid-based copolymer.

5. A method for producing a (meth)acrylic acid-based copolymer according to any one of claims 1 to 4, comprising the steps of: a preparation step of preparing a monomer mixture containing the monomer (ma), the monomer (mb), the monomer (mc) and water; and a polymerization step of continuously supplying the monomer mixture, a polymerization initiator, and an optional chain transfer agent to a reactor, respectively, and polymerizing the monomers.

6. The method for producing a (meth)acrylic acid-based copolymer according to claim 5, wherein in the polymerization step, the monomer mixture is supplied to the reactor for a time period of 2 to 12 hours.

7. A method for producing a (meth)acrylic acid-based copolymer described in claim 5 or 6, wherein in the polymerization process, polymerization of the monomer is carried out while maintaining the residual concentration of the monomer (mc) in the reactor at a total of 0.3 g / 100 mL or less.

8. A water treatment agent containing the (meth)acrylic acid copolymer according to any one of claims 1 to 4.

9. An anti-adhesion agent for calcium phosphate scale, calcium carbonate scale, calcium sulfate scale and silica scale, comprising the (meth)acrylic acid-based copolymer according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Preparation method of high-efficient copolymer silicon scale inhibitor

    CN108640299A

  • Scale preventive for water system

    JP1988107800A

  • Composition and method of preventing calcium phosphonate scale precipitate

    JP1988137799A

  • Metal corrosion preventive agent and metal corrosion preventive method

    JP1995268666A

  • Corrosion preventive dispersant and corrosion preventing method

    JP2001152372A