Easily thermally decomposable resin composition, molded article, packaging container, and method for chemically recycling thermoplastic resin

The integration of a solid acid catalyst in the thermoplastic resin composition facilitates energy-efficient thermal decomposition, addressing the energy intensity and catalyst replenishment challenges in existing recycling methods, enabling more efficient chemical recycling of thermoplastic resins.

WO2024203344A1PCT designated stage expired Publication Date: 2024-10-03TOYO SEIKAN GRP HLDG LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009814
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-13
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Chemical recycling of thermoplastic resins through thermal decomposition is energy-intensive and requires frequent catalyst replenishment, leading to increased costs and complex process management.

Method used

A thermoplastic resin composition incorporating a solid acid catalyst with acid catalytic activity at temperatures lower than the resin's thermal decomposition start, allowing for energy-efficient thermal decomposition and reducing the need for continuous catalyst replenishment.

Benefits of technology

The composition enables easier and more energy-efficient chemical recycling of thermoplastic resins by lowering the thermal decomposition initiation temperature, thereby reducing energy consumption and simplifying process management.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024009814_03102024_PF_FP_ABST
    Figure JP2024009814_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an easily thermally decomposable resin composition comprising a thermoplastic resin and a solid acid catalyst, wherein the solid acid catalyst exhibits an acid catalyst activity at a temperature lower by 10°C or more than the thermal decomposition initiation temperature of the thermoplastic resin.
Need to check novelty before this filing date? Find Prior Art

Description

Easily thermally decomposable resin composition, molded body, packaging container, and chemical recycling method for thermoplastic resin

[0001] The present invention relates to a thermally decomposable resin composition, a molded article, a packaging container, and a method for chemically recycling a thermoplastic resin.

[0002] Chemical recycling through pyrolysis is attracting attention as a way to realize horizontal recycling of general plastic products. Anaerobic pyrolysis is an endothermic reaction that requires a large amount of energy, so the combustion energy of pyrolysis gas is used, but this leads to the problem of emitting carbon dioxide.

[0003] One method for solving this problem is a thermal decomposition process using a solid acid catalyst (see, for example, Patent Document 1). In the catalytic decomposition method for waste plastics described in Patent Document 1, the waste plastics are catalytically decomposed and gasified by being introduced into a reactor containing a fluid catalyst cracking (FCC) catalyst.

[0004] Patent Document 1: Japanese Patent Application Laid-Open No. 2010-013657

[0005] However, the method described in Patent Document 1 requires continuous addition of new catalyst to compensate for the decrease in activity that occurs with the use and regeneration of the catalyst, which complicates process management and increases running costs. Therefore, there is a need for a method that can utilize the catalyst more efficiently.

[0006] An object of the present invention is to provide a thermally decomposable resin composition that enables easier and more energy-efficient chemical recycling of thermoplastic resins, a molded article made from such a thermally decomposable resin composition, a packaging container made from the molded article, and a method for chemically recycling thermoplastic resins.

[0007] The present inventors have found that the above object can be achieved by a thermally decomposable resin composition containing a thermoplastic resin and a solid acid catalyst, in which the solid acid catalyst exhibits acid catalytic activity at a temperature that is at least 10°C lower than the thermal decomposition onset temperature of the thermoplastic resin, and have completed the present invention.

[0008] [1] That is, according to a first aspect of the present invention, there is provided a thermally decomposable resin composition comprising a thermoplastic resin and a solid acid catalyst, wherein the solid acid catalyst exhibits acid catalytic activity at a temperature that is 10°C or more lower than the thermal decomposition onset temperature of the thermoplastic resin.

[0009] [2] According to a second aspect of the present invention, there is provided the thermally decomposable resin composition of the first aspect, wherein the solid acid catalyst is a proton-type or ammonium-type aluminosilicate.

[0010] [3] According to a third aspect of the present invention, there is provided the thermally decomposable resin composition according to the first or second aspect, wherein the thermoplastic resin is a polyolefin resin or a polyester resin.

[0011] [4] According to a fourth aspect of the present invention, there is provided the thermally decomposable resin composition according to any one of the first to third aspects, wherein the content of the solid acid catalyst is 0.1 to 30 wt %.

[0012] [5] According to a fifth aspect of the present invention, there is provided the thermally decomposable resin composition according to any one of the first to fourth aspects, wherein the solid acid catalyst is a spent catalyst.

[0013] [6] According to a sixth aspect of the present invention, there is provided the thermally decomposable resin composition according to any one of the first to fifth aspects, wherein the solid acid catalyst is composited in the thermoplastic resin.

[0014] [7] According to a seventh aspect of the present invention, there is provided a thermally decomposable resin composition according to any one of the first to sixth aspects, which is used in a recycling process.

[0015] [8] According to an eighth aspect of the present invention, there is provided a molded article made of the heat-decomposable resin composition of any one of the first to seventh aspects.

[0016] [9] According to a ninth aspect of the present invention, there is provided a packaging container comprising the molded article of the eighth aspect.

[0017]

[10] According to a tenth aspect of the present invention, there is provided a method for chemically recycling a thermoplastic resin, comprising the steps of: supplying the thermoplastic resin and the solid acid catalyst to an extruder to produce the thermally decomposable resin composition of any one of the first to seventh aspects; and thermally decomposing the thermally decomposable resin composition.

[0018] According to the easily thermally decomposable resin composition of the present invention, chemical recycling of thermoplastic resins can be carried out more simply and with more energy savings.

[0019] FIG. 1 is a graph showing the results of thermogravimetric analysis in Example 5 of the present invention and Comparative Example 1.

[0020] <Thermal Decomposition Resin Composition> The thermal decomposition resin composition of the present invention contains a thermoplastic resin and a solid acid catalyst, and the solid acid catalyst exhibits acid catalytic activity at a temperature that is 10°C or more lower than the thermal decomposition onset temperature of the thermoplastic resin.

[0021] <Thermoplastic Resin> Examples of the thermoplastic resin used in the present invention include polyolefin resins, polyester resins, polyamide resins, polystyrene resins, vinyl chloride resins, vinyl acetate resins, ABS resins, acrylic resins, acetal resins, polycarbonate resins, etc. These resins may be used alone, or multiple types may be used in combination by techniques such as blending or copolymerization. Among these, polyolefin resins or polyester resins are preferred from the viewpoint of further enhancing the effect of the solid acid catalyst of the present invention.

[0022] Examples of polyolefin resins include ethylene copolymer resins such as low-density polyethylene, linear low-density polyethylene, high-density polyethylene, ultra-high-density polyethylene, ethylene-vinyl alcohol copolymer, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-methyl acrylate copolymer; polyolefin elastomers such as polypropylene and ethylene-propylene block copolymer; etc. These resins may be used alone, or multiple types may be used in combination by blending, copolymerization, or the like.

[0023] Examples of polyester resins include polyethylene terephthalate resin, polyethylene naphthalate resin, polybutylene terephthalate resin, polybutylene naphthalate resin, polytrimethylene terephthalate resin, polytrimethylene naphthalate resin, polycyclohexane dimethyl terephthalate resin, etc. These resins may be used alone or in combination by blending or copolymerizing a plurality of types.

[0024] The content of the thermoplastic resin in the easily thermally decomposable resin composition is preferably 70 to 99.9% by weight, more preferably 80 to 99.9% by weight, and even more preferably 90 to 99.9% by weight.

[0025] The thermal decomposition starting temperature of the thermoplastic resin depends on the type of thermoplastic resin and is not particularly limited, but is preferably 200 to 600°C, more preferably 300 to 500°C.

[0026] <Solid Acid Catalyst> The solid acid catalyst is not particularly limited as long as it exhibits acid catalytic activity at a temperature 10°C or more lower than the thermal decomposition onset temperature of the thermoplastic resin. Examples include aluminosilicates, silica-alumina, and strongly acidic ion exchange resins. Among these, aluminosilicates are preferred. The temperature at which the solid acid catalyst exhibits acid catalytic activity is 10°C or more lower, preferably 40°C or more lower, than the thermal decomposition onset temperature of the thermoplastic resin. In the present invention, the thermal decomposition onset temperature refers to the temperature at which a weight loss of 5% by weight occurs by thermogravimetry. By measuring the thermal decomposition onset temperature of the thermally decomposable resin composition, it can be considered that the acid catalytic activity of the solid acid catalyst is exhibited at the thermal decomposition onset temperature. Therefore, if the thermal decomposition onset temperature measured for the thermally decomposable resin composition is 10°C or more lower than the thermal decomposition onset temperature measured for the thermoplastic resin alone, it can be determined that the solid acid catalyst exhibits acid catalytic activity at a temperature 10°C or more lower than the thermal decomposition onset temperature of the thermoplastic resin.

[0027] Aluminosilicates are compounds of the general formula M x/n [(AlO 2 ) x (SiO 2 ) y ]・zH2 O, and M is a cation having a valence of n. Examples of the cationic species include lithium ions, sodium ions, potassium ions, calcium ions, magnesium ions, barium ions, hydrogen ions, and ammonium ions, and the composition may contain a plurality of cationic species. From the viewpoint of further reducing the thermal decomposition onset temperature of the heat-decomposable resin composition of the present invention, the cationic species are preferably hydrogen ions (protons) and ammonium ions (NH 4 That is, as the aluminosilicate, proton type and ammonium type aluminosilicates are preferred.

[0028] Proton-type aluminosilicates are obtained by acid treating aluminosilicates whose cation species is a metal ion such as sodium ion, and exhibit acid catalytic activity at temperatures above room temperature. Ammonium-type aluminosilicates are obtained by ion exchange treatment of aluminosilicates whose cation species is a metal ion. Although ammonium-type aluminosilicates do not exhibit acid catalytic activity as they are, heating them to 250°C or higher causes ammonia elimination, resulting in the formation of proton-type aluminosilicates, which exhibit acid catalytic activity. A heat-decomposable resin composition containing an ammonium-type aluminosilicate as a solid acid catalyst is more suitable for processing into molded articles, due to the characteristic of ammonium-type aluminosilicates that they do not exhibit acid catalytic activity at melt-molding temperatures.

[0029] Examples of aluminosilicates represented by the general formula above include clay ores such as montmorillonite, zeolite, mullite, kaolinite, illite, and feldspar, as well as clays containing these as their main components. Clays containing montmorillonite as their main component include bentonite, acid clay, activated clay, and diatomaceous earth. Of these, activated clay, which is a proton-type aluminosilicate, is preferred. Aluminosilicates may be used alone or in combination. Furthermore, as long as the solid acid catalytic activity of the aluminosilicate is exhibited, other elements, metals, metal oxides, etc. may be supported on the aluminosilicate alone or in combination.

[0030] Zeolites include natural zeolites, synthetic zeolites, and artificial zeolites, and among these, synthetic zeolites and artificial zeolites are preferred. Zeolites may contain a variety of cation species, such as lithium ions, sodium ions, potassium ions, calcium ions, magnesium ions, barium ions, hydrogen ions, and ammonium ions, and may contain a plurality of cation species. From the viewpoint of further reducing the thermal decomposition initiation temperature of the heat-decomposable resin composition of the present invention, ammonium ions are preferred as the cation species of the zeolite. Zeolites containing ammonium ions as the cation species can be synthesized by ion-exchange treatment of zeolites.

[0031] Zeolite skeletal structures include A-type, X-type, beta-type, ferrierite, MCM-22, ZSM-5, mordenite, L-type, etc., and among these, ZSM-5 is preferred. The pore size of zeolite is derived from the skeletal structure and is not particularly limited, but is preferably 0.2 to 15 Å.

[0032] The particle size of the aluminosilicate is not particularly limited, but is preferably 1 to 1000 μm, more preferably 5 to 500 μm, and even more preferably 10 to 100 μm. The particle size of the aluminosilicate is not particularly limited, but can be measured by observing a cross section of the heat-decomposable resin composition with a scanning electron microscope or the like.

[0033] As mentioned above, proton-type aluminosilicates and ammonium-type aluminosilicates are preferably used as the solid acid catalyst, but are not particularly limited thereto. For example, a waste catalyst such as a waste FCC catalyst made of an aluminosilicate such as activated clay used in a petroleum fluid catalytic cracking process, or a waste catalyst such as waste clay generated during the production of fats and oils such as edible oil and mineral oil, may be used as the solid acid catalyst. The waste catalyst may be used alone as the solid acid catalyst, or may be regenerated by ignition and used, or may be used in combination with an unused solid acid catalyst.

[0034] The content of the solid acid catalyst in the thermally decomposable resin composition is preferably 0.1 to 30 wt %, more preferably 0.1 to 20 wt %, and even more preferably 0.1 to 10 wt %. Furthermore, the content of the solid acid catalyst relative to 100 parts by weight of the thermoplastic resin is preferably 1 to 45 parts by weight, more preferably 1 to 25 parts by weight, and even more preferably 1 to 10 parts by weight. By keeping the content of the solid acid catalyst within the above range, the thermal decomposition onset temperature of the thermally decomposable resin composition can be effectively reduced, thereby achieving energy savings in chemical recycling of the thermoplastic resin and reducing the amount of solid acid catalyst used. The method for measuring the content of the solid acid catalyst is not particularly limited. However, when a proton-type or ammonium-type aluminosilicate is used as the solid acid catalyst, the content can be determined by performing elemental analysis on the thermally decomposable resin composition to measure the proportions of silica and alumina.

[0035] The thermally decomposable resin composition may contain, in addition to the thermoplastic resin and the solid acid catalyst, known additives used in plastic products. Examples of additives include antioxidants, metal deactivators, flame retardants, antiaging agents, lubricants, fillers, reinforcing agents, UV absorbers, stabilizers, plasticizers, pigments, dyes, colorants, antistatic agents, and foaming agents. The content of the additives is not particularly limited as long as it does not impair the effects of the present invention, and can be adjusted depending on the purpose.

[0036] As the antioxidant, known antioxidants used in thermoplastic resins, etc., can be used, such as radical chain inhibitors such as phenolic antioxidants and amine antioxidants, peroxide decomposers such as phosphorus-based antioxidants and sulfur-based antioxidants, and metal deactivators such as hydrazine-based antioxidants and amine-based antioxidants. The antioxidants may be used alone or in combination. The amount of antioxidant used is not particularly limited, but the amount added may be adjusted appropriately taking into account the antioxidant effect and problems due to bleed-out.

[0037] The flame retardant is not particularly limited, and examples thereof include phosphorus-based flame retardants and non-phosphorus-based, non-halogen flame retardants such as metal hydrates. Phosphorus-based flame retardants include aluminum tris(diethylphosphinate), bisphenol A bis(diphenyl phosphate), triarylisopropyl phosphate, cresyl di-2,6-xylenyl phosphate, and aromatic condensed phosphate esters. Metal hydrates include aluminum trihydrate, magnesium dihydroxide, and combinations thereof. These may be used alone or in combination of two or more. Furthermore, antimony oxides such as antimony trioxide and antimony pentoxide, zinc oxide, iron oxide, aluminum oxide, molybdenum oxide, titanium oxide, calcium oxide, and magnesium oxide may also be used as auxiliary flame retardants. From the perspective of reducing environmental impact, it is preferable not to use halogen-based flame retardants.

[0038] <Method for Producing a Thermally Decomposable Resin Composition> The thermally decomposable resin composition of the present invention can be produced as a composite (composite material) by kneading and extruding a thermoplastic resin, a solid acid catalyst, and optional additives in a kneading extruder to uniformly mix and physically combine the components. The kneading temperature is not particularly limited as long as it is equal to or lower than the thermal decomposition onset temperature of the thermoplastic resin, but is preferably 120 to 350°C, and more preferably 150 to 300°C. By producing the thermally decomposable resin composition as a composite containing a thermoplastic resin and a solid acid catalyst, the decrease in the thermal decomposition onset temperature per amount of solid acid catalyst used (the difference between the thermal decomposition onset temperature of the thermoplastic resin alone and the thermal decomposition onset temperature when the catalyst is used) can be made greater than when the thermoplastic resin is simply contacted with the solid acid catalyst. In other words, by forming the thermally decomposable resin composition into a composite, the energy required for thermal decomposition can be efficiently reduced.

[0039] The thermally decomposable resin composition of the present invention contains a solid acid catalyst, which reduces the thermal decomposition onset temperature and reduces the energy required for thermal decomposition. Therefore, the thermally decomposable resin composition of the present invention can achieve energy savings in chemical recycling of thermoplastic resins. Furthermore, because the thermally decomposable resin composition of the present invention contains a solid acid catalyst, it can be thermally decomposed without the need to supply a separate catalyst in the thermal decomposition process. This makes it possible to more easily chemically recycle thermoplastic resins.

[0040] The thermally decomposable resin composition of the present invention can be suitably used in the chemical recycling of waste plastics made from thermoplastic resins. For example, waste plastics made from thermoplastic resins can be kneaded with a solid acid catalyst to form a composite to obtain the thermally decomposable resin composition of the present invention, which can then be heated and pyrolyzed to produce cracked oil or cracked gas. Methods for supplying the thermally decomposable resin composition to the pyrolysis process include supplying it as a molded product such as pellets or powder, or supplying it in a molten state. The pyrolysis method is not particularly limited, but it can be carried out by heating the thermally decomposable resin composition in an oxygen-free or low-oxygen atmosphere in a reactor such as a stirred tank, rotary kiln, packed bed, or fluidized bed. The temperature can be selected from the range of 300 to 1500°C, with 300 to 600°C being particularly preferred. By pyrolyzing the thermally decomposable resin composition at 300 to 600°C, many of the recovered components can be recovered as cracked oil, which can be supplied to existing chemical manufacturing processes as a replacement for crude oil or its fractions. The obtained cracked oil is converted into basic chemical raw materials through known processing steps for petroleum refining and chemical raw material production, i.e., desulfurization, desalting, hydrogenation, distillation, purification, hydrothermal cracking, catalytic cracking, catalytic reforming, etc. The basic chemical raw materials obtained in this manner can be chemically recycled by repolymerizing them and processing them into plastic products. When the thermally decomposable resin composition of the present invention is used for the thermal decomposition of waste plastics, it is preferable to use a proton-type aluminosilicate such as activated clay as the solid acid catalyst, from the viewpoint of further reducing the thermal decomposition onset temperature of the thermally decomposable resin composition.

[0041] The heat-decomposable resin composition of the present invention is also suitable for processing into molded articles imparted with heat decomposability. Molded articles obtained by processing the heat-decomposable resin composition of the present invention are imparted with heat decomposability due to the inclusion of a solid acid catalyst, and can be thermally decomposed while saving energy, making them suitable for chemical recycling. The molded articles can be applied to a wide range of applications in which plastics are typically used. In particular, the composition is suitable for applications in which material recycling is difficult due to the composite material, the significant contamination with other components that occurs with use, and the high cleanliness requirements for the raw materials used. From this perspective, the composition is also suitable for use in food packaging containers made of composite materials. When the heat-decomposable resin composition of the present invention is used for molded articles, it is preferable to use an ammonium-type aluminosilicate, such as zeolite, as the solid acid catalyst, in order to suppress thermal decomposition of the solid acid catalyst during the production of the heat-decomposable resin composition and to ensure a favorable appearance of the molded article.

[0042] Next, the present invention will be specifically explained by way of examples, but the present invention is not limited to these examples.

[0043] Example 1 (Preparation of Composite) 90 parts by weight of pelletized low-density polyethylene (LDPE) (product name "Sumikathen G-201F", manufactured by Sumitomo Chemical Co., Ltd.) and 10 parts by weight of activated clay (proton-type aluminosilicate) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a solid acid catalyst were added to and kneaded with a twin-screw kneading extruder (product name "ULTnano", manufactured by Technovel Co., Ltd.) equipped with powder supply equipment and granulation equipment, to obtain a composite (pellet) of a heat-decomposable resin composition. The composition of the composite is shown in Table 1.

[0044] (Measurement of Thermal Decomposition Onset Temperature) The obtained composite was subjected to thermogravimetric measurement using a differential thermal analyzer (product name "STA7200RV", manufactured by Hitachi High-Tech Science Corporation). The measurement was carried out under conditions of a nitrogen flow rate of 200 mL / min, a temperature range of 40 to 540°C, and a heating rate of 10°C / min. The temperature at which a weight loss of 5 wt% of the initial weight of the composite occurred was defined as the thermal decomposition onset temperature. Since the weight of the composite decreased and the thermal decomposition onset temperature was measured, it was confirmed that the solid acid catalyst contained in the composite exhibited acid catalytic activity at the thermal decomposition onset temperature. The results are shown in Table 2.

[0045] (Decrease in thermal decomposition onset temperature per amount of solid acid catalyst added component) The difference between the thermal decomposition onset temperature of the thermally decomposable resin composition and the thermal decomposition onset temperature measured for the thermoplastic resin alone was divided by the amount (wt%) of solid acid catalyst added to the thermally decomposable resin composition to calculate the decrease in thermal decomposition onset temperature (°C) per amount of solid acid catalyst added component. The thermal decomposition onset temperature measured for the thermoplastic resin alone was the thermal decomposition onset temperature measured in Comparative Example 1 described below.

[0046] [Examples 2 to 4] Composites of thermally decomposable resin compositions were obtained and evaluated in the same manner as in Example 1, except that the amounts of low-density polyethylene and activated clay were changed to those shown in Table 1. The results are shown in Tables 1 and 2.

[0047] Examples 5 to 7 Composites of thermally decomposable resin compositions were obtained and evaluated in the same manner as in Example 1, except that ZSM-5 zeolite (pore diameter: 5.6 Å, ammonium aluminosilicate) (ZSM-5 ammonium: manufactured by Thermo Scientific) was used as the solid acid catalyst instead of activated clay, and the amounts of low-density polyethylene and zeolite used were set as shown in Table 1. The results are shown in Tables 1 and 2.

[0048] Example 8 A composite of a thermally decomposable resin composition was obtained and evaluated in the same manner as in Example 1, except that pelletized homopolypropylene (homoPP) (product name "Prime Polypro E-200GP", manufactured by Prime Polymer Co., Ltd.) was used instead of low-density polyethylene. The results are shown in Tables 1 and 2. When calculating the temperature decrease in thermal decomposition onset temperature per amount of solid acid catalyst added component, the thermal decomposition onset temperature measured in Comparative Example 2, which will be described later, was used as the thermal decomposition onset temperature measured for the thermoplastic resin alone.

[0049] Example 9 A composite of a thermally decomposable resin composition was obtained and evaluated in the same manner as in Example 1, except that pelletized polyethylene terephthalate (PET) (product name "5015W", manufactured by Shinko Synthetic Fibers Co., Ltd.) was used instead of low-density polyethylene. The results are shown in Tables 1 and 2. When calculating the temperature decrease in thermal decomposition onset temperature per amount of solid acid catalyst added component, the thermal decomposition onset temperature measured in Comparative Example 8, which will be described later, was used as the thermal decomposition onset temperature measured for the thermoplastic resin alone.

[0050] Comparative Example 1 Pellets consisting of only low-density polyethylene were obtained in the same manner as in Example 1, except that activated clay was not added as a solid acid catalyst. Thermogravimetry of the low-density polyethylene pellets was carried out under the same conditions as in Example 1. The results are shown in Table 2.

[0051] Comparative Example 2 Pellets consisting of homopolypropylene alone were obtained in the same manner as in Example 8, except that activated clay was not added as a solid acid catalyst. Thermogravimetry of the homopolypropylene pellets was carried out under the same conditions as in Example 1. The results are shown in Table 2.

[0052] Comparative Example 3 A composite of a thermally decomposable resin composition was obtained and evaluated in the same manner as in Example 2, except that montmorillonite (sodium aluminosilicate) (product name "PGW", manufactured by Volclay Co., Ltd.) was used instead of activated clay. The results are shown in Tables 1 and 2.

[0053] Comparative Example 4 A composite of a thermally decomposable resin composition was obtained and evaluated in the same manner as in Example 2, except that A-type zeolite (pore diameter: 3 Å, sodium, potassium-type aluminosilicate) (molecular sieve 3A powder, manufactured by Union Showa Co., Ltd.) was used instead of activated clay, and the amounts of low-density polyethylene and zeolite used were as shown in Table 1. The results are shown in Tables 1 and 2.

[0054] Comparative Example 5 A composite of a thermally decomposable resin composition was obtained and evaluated in the same manner as in Example 8, except that montmorillonite was used instead of activated clay and the amounts of homopolypropylene and montmorillonite used were as shown in Table 1. The results are shown in Tables 1 and 2.

[0055] Comparative Example 6 Low-density polyethylene and activated clay were placed on the aluminum pan of a differential thermal thermogravimetric analyzer in a weight ratio of 1:1, and thermogravimetric measurement was carried out under the same conditions as in Example 1. The results are shown in Table 2.

[0056] Comparative Example 7 Low-density polyethylene and ZSM-5 zeolite were placed on the aluminum pan of a differential thermal thermogravimetry apparatus in a weight ratio of 1:1, and thermogravimetry was carried out under the same conditions as in Example 1. The results are shown in Table 2.

[0057] Comparative Example 8 Pellets consisting of only polyethylene terephthalate were obtained in the same manner as in Example 9, except that activated clay was not added as a solid acid catalyst. Thermogravimetry of the polyethylene terephthalate pellets was carried out under the same conditions as in Example 1. The results are shown in Table 2.

[0058]

[0059]

[0060] As shown in Table 2, the thermally decomposable resin composition containing a thermoplastic resin and a solid acid catalyst exhibited a lower thermal decomposition onset temperature than the composition without the solid acid catalyst (Comparative Examples 1, 2, and 8), demonstrating the ability to reduce the energy required for thermal decomposition (see Figure 1). Figure 1 is a graph showing the results of thermogravimetric analysis for Example 5 and Comparative Example 1. Furthermore, as is clear from a comparison of Examples 1 to 8 with Comparative Examples 6 and 7, the addition of a solid acid catalyst to a thermoplastic resin to form a composite resulted in a greater reduction in the thermal decomposition onset temperature per amount of solid acid catalyst used than when the catalyst was simply contacted with the thermoplastic resin, demonstrating the ability to efficiently reduce the energy required for thermal decomposition. The reduction in the thermal decomposition onset temperature for Examples 1 to 7, which used low-density polyethylene, was calculated by dividing the reduction in the thermal decomposition onset temperature relative to the thermal decomposition onset temperature of Comparative Example 1, which used low-density polyethylene alone, by the amount of added components. The reduction in the thermal decomposition onset temperature for Example 8, which used homopolypropylene, was calculated by dividing the reduction in the thermal decomposition onset temperature relative to the thermal decomposition onset temperature of Comparative Example 2, which used homopolypropylene alone, by the amount of added components.

[0061] Furthermore, as shown in Table 1, the composite using an ammonium-type aluminosilicate as the solid acid catalyst exhibited a white appearance, indicating that it can also be suitably used as a molded product imparted with thermal decomposition properties.

Claims

1. A thermally decomposable resin composition comprising a thermoplastic resin and a solid acid catalyst, wherein the solid acid catalyst exhibits acid catalytic activity at a temperature that is at least 10°C lower than the thermal decomposition onset temperature of the thermoplastic resin.

2. The easily thermally decomposable resin composition according to claim 1, wherein the solid acid catalyst is a proton type or ammonium type aluminosilicate.

3. The easily thermally decomposable resin composition according to claim 1 or 2, wherein the thermoplastic resin is a polyolefin resin or a polyester resin.

4. The easily thermally decomposable resin composition according to any one of claims 1 to 3, wherein the content of the solid acid catalyst is 0.1 to 30% by weight.

5. The easily thermally decomposable resin composition according to any one of claims 1 to 4, wherein the solid acid catalyst is a waste catalyst.

6. The easily thermally decomposable resin composition according to any one of claims 1 to 5, wherein the solid acid catalyst is composited in the thermoplastic resin.

7. The easily thermally decomposable resin composition according to any one of claims 1 to 6, which is used in a recycling process.

8. A molded article made of the heat-decomposable resin composition according to any one of claims 1 to 7.

9. A packaging container comprising the molded article according to claim 8.

10. A method for chemically recycling a thermoplastic resin, comprising the steps of: supplying the thermoplastic resin and the solid acid catalyst to an extruder to produce the thermally decomposable resin composition according to claim 1 or 2; and thermally decomposing the thermally decomposable resin composition.

Citation Information

Patent Citations

  • Easily thermally decomposable plastic composition and molded item

    JP1997291171A

  • Method for liquefying cellulose-based biomass

    JP2009296919A

  • Thermoplastic resin composition and molded artifact of the same

    JP2014031409A

  • Deodorant film

    JP2020163017A