Crosslinked elastomer composition, production method for same, adhesive sheet, laminated glass, and electrical / electronic sealing material

The crosslinked elastomer composition, formed by modifying hydrogenated block copolymers with alkoxysilyl groups and specific catalysts, addresses the heat and solvent resistance issues in adhesive sheets, providing enhanced performance for laminated glass and electronic encapsulants.

WO2024203358A1PCT designated stage expired Publication Date: 2024-10-03ZEON CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009887
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-13
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional crosslinked elastomers used in adhesive sheets for laminated glass lack sufficient heat resistance and solvent resistance, particularly when exposed to temperatures and solvents like toluene and cyclohexane.

Method used

A crosslinked elastomer composition is developed by introducing an alkoxysilyl group into a hydrogenated block copolymer containing structural units from aromatic vinyl compounds and chain conjugated diene compounds, and further crosslinking it with a condensation catalyst such as titanium (IV) acetylacetonate, maleic acid, or succinic acid, to enhance adhesion and elongation properties.

Benefits of technology

The resulting adhesive sheet exhibits excellent heat resistance and solvent resistance, maintaining flexibility across a wide temperature range and resisting dissolution in solvents, making it suitable for laminated glass and electrical/electronic encapsulants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided is a crosslinked elastomer composition comprising a crosslinked elastomer that is obtained by crosslinking a modified block copolymer hydride, wherein: the modified block copolymer hydride is obtained by introducing an alkoxysilyl group into a hydride of a block copolymer containing a structural unit which is derived from an aromatic vinyl compound and a structural unit which is derived from a chain conjugated diene compound; and regarding the dynamic viscoelasticity of the crosslinked elastomer composition measured on the basis of JIS K7244-2, the peak top temperature of tanδ is -70 to -35°C.
Need to check novelty before this filing date? Find Prior Art

Description

Crosslinked elastomer composition and its manufacturing method, adhesive sheet, laminated glass, and sealing material for electrical and electronic applications

[0001] The present invention relates to a crosslinked elastomer composition and a method for producing the same, an adhesive sheet, laminated glass, and an electrical and electronic sealing material.

[0002] BACKGROUND ART Crosslinked elastomers obtained by crosslinking hydrogenated block copolymers and / or modified products thereof have conventionally been used as materials for adhesive sheets constituting interlayer films for laminated glass and the like.

[0003] For example, Patent Document 1 reports that an adhesive sheet having at least one layer made of a crosslinked elastomer having a tan δ peak in the temperature range of −20° C. to +20° C. in the dynamic viscoelastic properties measured according to JIS K7244-2 can be used to produce laminated glass with excellent sound insulation and heat resistance. Patent Document 1 also reports that a crosslinked elastomer that can be suitably used in the adhesive sheet can be obtained by crosslinking, in the presence or absence of a crosslinking coagent, a hydrogenated block copolymer [D] obtained by hydrogenating the carbon-carbon unsaturated bonds of a block copolymer [C] consisting of a polymer block [A] mainly composed of structural units derived from an aromatic vinyl compound and a polymer block [B] mainly composed of structural units derived from a linear conjugated diene compound, and / or a modified hydrogenated block copolymer [E] obtained by introducing alkoxysilyl groups into the hydrogenated block copolymer [D].

[0004] International Publication No. 2018 / 097146

[0005] Here, adhesive sheets using crosslinked elastomers are required to have excellent heat resistance and also to be difficult to dissolve in solvents such as toluene and cyclohexane, that is, to have excellent solvent resistance.

[0006] Therefore, an object of the present invention is to provide a crosslinked elastomer composition capable of forming an adhesive sheet having excellent heat resistance and solvent resistance. Another object of the present invention is to provide an adhesive sheet having excellent heat resistance and solvent resistance. A further object of the present invention is to provide laminated glass comprising the above adhesive sheet. And a final object of the present invention is to provide an electrical and electronic sealing material comprising the above crosslinked elastomer composition.

[0007] The present inventors have conducted extensive research with the aim of solving the above-mentioned problems, and have newly discovered that an adhesive sheet with excellent heat resistance and solvent resistance can be formed using an elastomer composition that includes a crosslinked elastomer obtained by further crosslinking a modified hydrogenated block copolymer in which an alkoxysilyl group has been introduced into a hydrogenated block copolymer containing structural units derived from an aromatic vinyl compound and structural units derived from a linear conjugated diene compound, and that has a peak top temperature of tan δ in dynamic viscoelasticity within a specified range, thereby completing the present invention.

[0008] That is, the object of the present invention is to advantageously solve the above-mentioned problems, and the present invention provides the following crosslinked elastomer compositions [1] to [4], methods for producing crosslinked elastomer compositions [5] to [7], adhesive sheets [8], laminated glass [9], and electrical and electronic sealing materials

[10] .

[0009] [1] A crosslinked elastomer composition comprising a crosslinked elastomer obtained by crosslinking a modified hydrogenated block copolymer, wherein the modified hydrogenated block copolymer is a hydrogenated block copolymer containing structural units derived from an aromatic vinyl compound and structural units derived from a linear conjugated diene compound, to which an alkoxysilyl group has been introduced, and wherein the crosslinked elastomer composition has a dynamic viscoelasticity measurement tan δ peak-top temperature of −70° C. to −35° C. as measured in accordance with JIS K7244-2. Thus, an elastomer composition comprising a crosslinked elastomer obtained by further crosslinking a modified hydrogenated block copolymer containing structural units derived from an aromatic vinyl compound and structural units derived from a linear conjugated diene compound, to which an alkoxysilyl group has been introduced, and having a dynamic viscoelasticity measurement tan δ peak-top temperature within a predetermined range, can be used to form an adhesive sheet with excellent heat resistance and solvent resistance. In the present invention, the peak top temperature of tan δ in dynamic viscoelasticity measured based on JIS K7244-2 and the value of tan δ at the peak top temperature can be measured using the method described in the examples of this specification.

[0010] [2] The crosslinked elastomer composition according to [1] above, wherein the modified hydrogenated block copolymer is a hydrogenated block copolymer [D] obtained by hydrogenating carbon-carbon unsaturated bonds of a block copolymer [C] comprising at least two polymer blocks [A] mainly composed of structural units derived from an aromatic vinyl compound and at least one polymer block [B] mainly composed of structural units derived from a chain-like conjugated diene compound, and wherein an alkoxysilyl group is introduced into the hydrogenated block copolymer [D], and wherein the mass fraction of all polymer blocks [A] in the block copolymer [C] relative to the entire block copolymer [C] is wA, and the mass fraction of all polymer blocks [B] in the block copolymer [C] relative to the entire block copolymer [C] is wB, and the ratio of wA to wB (wA:wB) is 30:70 to 60:40.

[0011] [3] The crosslinked elastomer composition according to [1] or [2] above, wherein the crosslinked elastomer is obtained by crosslinking the hydrogenated modified block copolymer in the presence of a condensation catalyst, and the condensation catalyst contains at least one selected from the group consisting of a metal carboxylate, an organic titanium compound, an organic zirconium compound, an organic aluminum compound, an organic base, an inorganic acid, and an organic acid.

[0012] [4] The crosslinked elastomer composition according to [3], wherein the condensation catalyst comprises at least one of titanium (IV) acetylacetonate, maleic acid, and succinic acid. By using at least one of titanium (IV) acetylacetonate, maleic acid, and succinic acid as the condensation catalyst, the adhesive properties and elongation of the adhesive sheet obtained by molding the crosslinked elastomer composition can be improved.

[0013] [5] A method for producing a crosslinked elastomer composition according to any one of [1] to [4] above, comprising a crosslinking step of crosslinking the hydrogenated modified block copolymer in the presence of a condensation catalyst, wherein the condensation catalyst contains at least one selected from the group consisting of a metal carboxylate, an organic titanium compound, an organic zirconium compound, an organic aluminum compound, an organic base, an inorganic acid, and an organic acid.

[0014] [6] The method for producing a crosslinked elastomer composition according to [5] above, wherein the condensation catalyst contains at least one of titanium (IV) acetylacetonate, maleic acid, and succinic acid. By using at least one of titanium (IV) acetylacetonate, maleic acid, and succinic acid as the condensation catalyst, the adhesive properties and elongation of the adhesive sheet produced by molding the crosslinked elastomer composition can be improved.

[0015] [7] The method for producing a crosslinked elastomer composition according to [5] or [6] above, wherein the amount of the condensation catalyst used is 0.01 parts by mass or more and 5.00 parts by mass or less per 100 parts by mass of the modified hydrogenated block copolymer.

[0016] [8] An adhesive sheet obtained by molding the crosslinked elastomer composition according to any one of [1] to [4] above. The adhesive sheet obtained by molding the crosslinked elastomer composition of the present invention described above is excellent in both heat resistance and solvent resistance.

[0017] [9] Laminated glass comprising the adhesive sheet described in [8] above.

[0018]

[10] An electrical and electronic sealing material comprising the crosslinked elastomer composition according to any one of [1] to [4] above.

[0019] According to the present invention, a crosslinked elastomer composition capable of forming an adhesive sheet having excellent heat resistance and solvent resistance can be provided. Furthermore, according to the present invention, an adhesive sheet having excellent heat resistance and solvent resistance can be provided. Furthermore, according to the present invention, a laminated glass including the adhesive sheet can be provided. Finally, according to the present invention, an electrical and electronic sealing material including the above-described crosslinked elastomer composition can be provided.

[0020] Hereinafter, embodiments of the present invention will be described in detail. Here, the crosslinked elastomer composition of the present invention is used to form the adhesive sheet of the present invention. The crosslinked elastomer composition of the present invention is also included in the electrical and electronic sealant of the present invention. The adhesive sheet of the present invention can be used in various applications, including the production of the laminated glass and electrical and electronic sealant of the present invention.

[0021] (Crosslinked Elastomer Composition) The crosslinked elastomer composition of the present invention contains a crosslinked elastomer obtained by crosslinking a hydrogenated modified block copolymer, and optionally further contains components other than the crosslinked elastomer (hereinafter, sometimes referred to as "other components").

[0022] <Dynamic Viscoelasticity> The crosslinked elastomer composition of the present invention must have a peak top temperature of tan δ in dynamic viscoelasticity measured in accordance with JIS K7244-2 that is −70° C. or higher, preferably −65° C. or higher, more preferably −60° C. or higher, and even more preferably −55° C. or higher, and must be −35° C. or lower, preferably −40° C. or lower, and more preferably −45° C. or lower. If the peak top temperature of tan δ in the dynamic viscoelasticity of the crosslinked elastomer composition is within the above-mentioned specified range, an adhesive sheet obtained by molding the crosslinked elastomer composition will be able to achieve both flexibility and heat resistance over a wide temperature range.

[0023] The peak top temperature of tan δ in the dynamic viscoelasticity of the crosslinked elastomer composition and the value of tan δ at the peak top temperature are not particularly limited, but can be controlled, for example, by the proportion of structural units derived from a chain conjugated diene compound polymerized via 1,2-bonds and / or 3,4-bonds, among structural units derived from a chain conjugated diene compound in the block copolymer [C] used in producing the crosslinked elastomer.

[0024] <Solvent Resistance> The crosslinked elastomer composition of the present invention contains a crosslinked elastomer obtained by crosslinking a modified hydrogenated block copolymer, and therefore the adhesive sheet formed can exhibit sufficient solvent resistance. The solvent resistance of the crosslinked elastomer composition is preferably such that the residual rate when dissolved in toluene solvent, calculated using the method described in the Examples section of this specification, is 20% or more, and more preferably 30% or more. If the solvent resistance is at or above the lower limit, the solvent resistance is sufficient and the composition can be suitably used for various applications. The upper limit of the solvent resistance is not particularly limited and may be 100% (insoluble in toluene solvent) or, for example, 90% or less.

[0025] <Crosslinked Elastomer> In the present invention, the term "crosslinked elastomer" refers to a polymer compound that exhibits rubber elasticity within the above-mentioned range of the peak top temperature of tan δ. The crosslinked elastomer contained in the crosslinked elastomer composition of the present invention is a crosslinked product obtained by crosslinking a hydrogenated modified block copolymer as a precursor.

[0026] The content of the crosslinked elastomer in the crosslinked elastomer composition of the present invention is not particularly limited, but is usually 80% by mass or more, preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 99% by mass or more, and can be 100% by mass or less, assuming that the total mass of the crosslinked elastomer composition is 100% by mass.

[0027] <<Modified Hydrogenated Block Copolymer>> The modified hydrogenated block copolymer, which is a precursor of a crosslinked elastomer, is a modified product obtained by introducing an alkoxysilyl group into a hydrogenated block copolymer containing a structural unit derived from an aromatic vinyl compound (hereinafter sometimes referred to as "structural unit [a]") and a structural unit derived from a linear conjugated diene compound (hereinafter sometimes referred to as "structural unit [b]"). The modified hydrogenated block copolymer is preferably a modified hydrogenated block copolymer [E] obtained by introducing an alkoxysilyl group into a hydrogenated block copolymer [D] obtained by hydrogenating the carbon-carbon unsaturated bonds of a block copolymer [C] consisting of at least two polymer blocks [A] mainly composed of structural unit [a] derived from an aromatic vinyl compound and at least one polymer block [B] mainly composed of structural unit [b] derived from a linear conjugated diene compound. In the present invention, the phrase "mainly composed of" a specific structural unit means that "the polymer block contains 70% by mass or more of the structural unit, with all structural units (all repeating units) constituting the polymer block being 100% by mass."

[0028] [Block Copolymer [C]] The block copolymer [C] preferably has at least two polymer blocks [A] and at least one polymer block [B].

[0029] [Polymer Block [A]] Polymer block [A] is a polymer block primarily composed of structural unit [a] derived from an aromatic vinyl compound. The content of structural unit [a] in polymer block [A] must be 70% by mass or more, preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more, based on 100% by mass of all structural units constituting polymer block [A]. When the content of structural unit [a] in polymer block [A] is equal to or greater than the above-mentioned lower limit, the heat resistance of an adhesive sheet obtained by molding the crosslinked elastomer composition can be further improved. The upper limit of the content of structural unit [a] in polymer block [A] is not particularly limited, and can be 100% by mass or less.

[0030] The polymer block [A] may contain structural units (other structural units) other than the structural unit [a]. Examples of other structural units that the polymer block [A] may contain include the structural unit [b] derived from a chain conjugated diene compound and / or the structural unit [j] derived from other vinyl compounds. The total content of the structural unit [b] derived from a chain conjugated diene compound and the structural unit [j] derived from other vinyl compounds in the polymer block [A] must be 30% by mass or less, preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 2% by mass or less, based on 100% by mass of all structural units constituting the polymer block [A].

[0031] -Aromatic Vinyl Compound- Examples of aromatic vinyl compounds used to introduce the structural unit [a] include styrene; styrenes having an alkyl group having from 1 to 6 carbon atoms as a substituent, such as α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-diisopropylstyrene, 2,4-dimethylstyrene, 4-t-butylstyrene, and 5-t-butyl-2-methylstyrene; styrenes having an alkoxy group having from 1 to 6 carbon atoms as a substituent, such as 4-methoxystyrene; styrenes having an aryl group as a substituent, such as 4-phenylstyrene; and vinylnaphthalenes, such as 1-vinylnaphthalene and 2-vinylnaphthalene. These may be used alone or in combination of two or more. Among these, aromatic vinyl compounds not containing a polar group, such as styrene and styrenes having an alkyl group having from 1 to 6 carbon atoms as a substituent, are preferred from the viewpoint of reducing the moisture absorption of an adhesive sheet obtained by molding the crosslinked elastomer composition, and styrene is particularly preferred from the viewpoint of industrial ease of availability.

[0032] -Linear Conjugated Diene Compound- Furthermore, examples of linear conjugated diene compounds (linear conjugated diene compounds, branched conjugated diene compounds) used to introduce the structural unit [b] include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, chloroprene, etc. These may be used alone or in combination of two or more. Among these, from the viewpoint of reducing the moisture absorption of an adhesive sheet obtained by molding the crosslinked elastomer composition, linear conjugated diene compounds that do not contain a polar group are preferred, and 1,3-butadiene and isoprene are particularly preferred from the standpoint of industrial ease of availability.

[0033] Other vinyl compounds used to introduce the structural unit [j] include vinyl compounds other than aromatic vinyl compounds and chain conjugated diene compounds, such as chain vinyl compounds, cyclic vinyl compounds, unsaturated cyclic acid anhydrides, and unsaturated imide compounds. These compounds may have a substituent such as a nitrile group, an alkoxycarbonyl group, a hydroxycarbonyl group, or a halogen atom. These compounds may be used alone or in combination of two or more. Among these, from the viewpoint of reducing the moisture absorption of the molded body [F], preferred are those which do not contain a polar group, such as linear vinyl compounds (linear olefins) having from 2 to 20 carbon atoms, such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-dodecene, 1-eicosene, 4-methyl-1-pentene, and 4,6-dimethyl-1-heptene; cyclic vinyl compounds (cyclic olefins) having from 5 to 20 carbon atoms, such as vinylcyclohexane and norbornene; and cyclic diene compounds, such as 1,3-cyclohexadiene and norbornadiene.

[0034] [Polymer Block [B]] Polymer block [B] is a polymer block primarily composed of structural unit [b] derived from a linear conjugated diene compound. The content of structural unit [b] in polymer block [B] must be 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more, based on 100% by mass of all structural units constituting polymer block [B]. When the content of structural unit [b] in polymer block [B] is equal to or greater than the above-mentioned lower limit, the adhesiveness of an adhesive sheet obtained by molding the crosslinked elastomer composition can be improved. The upper limit of the content of structural unit [b] in polymer block [B] is not particularly limited, and can be 100% by mass or less.

[0035] The polymer block [B] may contain a structural unit (other structural unit) other than the structural unit [b]. Examples of other structural units that the polymer block [B] may contain include the structural unit [a] derived from an aromatic vinyl compound and / or the structural unit [j] derived from another vinyl compound, as described above in the section "Polymer block [A]." The total content of the structural unit [a] derived from an aromatic vinyl compound and the structural unit [j] derived from another vinyl compound in the polymer block [B] must be 30% by mass or less, preferably 20% by mass or less, and more preferably 10% by mass or less, based on 100% by mass of all structural units constituting the polymer block [B].

[0036] —Linear Conjugated Diene Compound, Aromatic Vinyl Compound, and Other Vinyl Compounds— Specific examples of the linear conjugated diene compound used to introduce the structural unit [b], the aromatic vinyl compound used to introduce the structural unit [a], and the other vinyl compound used to introduce the structural unit [j] include those described above in the section “Polymer Block [A],” and preferred examples of each are the same as those described as preferred examples in the section “Polymer Block [A].”

[0037] [Properties of Block Copolymer [C]] Here, when the mass fraction of the total amount of structural units [a] derived from aromatic vinyl compounds in the block copolymer [C] is wa, and the mass fraction of the total amount of structural units [b] derived from linear conjugated diene compounds in the block copolymer [C] is wb, the ratio of wa to wb (wa:wb) is preferably 30:70 to 60:40, more preferably 35:65 to 60:40, even more preferably 35:65 to 55:45, still more preferably 40:60 to 55:45, and even more preferably 45:55 to 55:45. By making the mass fraction (wa) of structural units [a] derived from aromatic vinyl compounds 30% or more, the heat resistance of adhesive sheets obtained by molding the crosslinked elastomer composition can be further improved. On the other hand, by setting the mass fraction (wa) of the structural unit [a] derived from the aromatic vinyl compound to 60% or less, the elongation of the adhesive sheet obtained by molding the crosslinked elastomer composition can be improved. Note that the "ratio of wa to wb (wa:wb)" can be calculated from the parts of the aromatic vinyl compound, linear conjugated diene compound, and other vinyl compounds used in the polymerization of the block copolymer in the process of producing the block copolymer, and the polymerization conversion rate of the monomers used to polymerize each block of the block copolymer at the end of the polymerization, measured using gas chromatography (GC).

[0038] Furthermore, when the mass fraction of all polymer blocks [A] in the block copolymer [C] relative to the entire block copolymer [C] is wA, and the mass fraction of all polymer blocks [B] relative to the entire block copolymer [C] is wB, the ratio of wA to wB (wA:wB) is preferably 30:70 to 60:40, more preferably 35:65 to 60:40, even more preferably 35:65 to 55:45, even more preferably 40:60 to 55:45, and even more preferably 45:55 to 55:45. By making the mass fraction (wA) of the polymer block [A] 30% or more, the heat resistance of the adhesive sheet obtained by molding the crosslinked elastomer composition can be further improved. On the other hand, by making the mass fraction (wA) of the polymer block [A] 60% or less, the elongation of the adhesive sheet obtained by molding the crosslinked elastomer composition can be improved. The "ratio of wA to wB (wA:wB)" can be calculated from the parts of the aromatic vinyl compound, the linear conjugated diene compound, and other vinyl compounds used in the polymerization of the block copolymer in the process of producing the block copolymer, and the polymerization conversion rate of the monomers used to polymerize each block of the block copolymer measured using gas chromatography (GC) at the end of the polymerization.

[0039] As described above, the number of polymer blocks [A] in the block copolymer [C] is preferably 2 or more, preferably 3 or less, and more preferably 2. As described above, the number of polymer blocks [B] in the block copolymer [C] is preferably 1 or more, preferably 2 or less, and more preferably 1.

[0040] The polymer blocks [A] contained in the block copolymer [C] may be identical to or different from each other in composition and / or block length. When the block copolymer [C] has a plurality of polymer blocks [B], the polymer blocks [B] may be identical to or different from each other in composition and / or block length.

[0041] The block form of the block copolymer [C] is not particularly limited, and may be a chain block or a radial block. From the viewpoint of improving the mechanical strength of the adhesive sheet obtained by molding the crosslinked elastomer composition, a chain block is preferred. The most preferred form of the block copolymer [C] is a triblock copolymer ([A]-[B]-[A]) in which the polymer block [A] is bonded to both ends of the polymer block [B].

[0042] The molecular weight of the block copolymer [C], as measured by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent, is preferably 25,000 or more, more preferably 30,000 or more, even more preferably 35,000 or more, and preferably 200,000 or less, more preferably 170,000 or less, as a weight average molecular weight (Mw) calculated in terms of polystyrene. When the weight average molecular weight (Mw) of the block copolymer [C] is within the above-mentioned range, the heat resistance of the adhesive sheet obtained by molding the crosslinked elastomer composition can be further improved. Furthermore, the molecular weight distribution (Mw / Mn) of the block copolymer [C] is preferably 3.0 or less, more preferably 2.0 or less, and particularly preferably 1.5 or less. When the molecular weight distribution (Mw / Mn) of the block copolymer [C] is within the above-mentioned range, the heat resistance of the adhesive sheet obtained by molding the crosslinked elastomer composition can be further improved.

[0043] In the block copolymer [C], a portion of the linear conjugated diene compound forms structural units polymerized via 1,2-bonds and / or 3,4-bonds (hereinafter, these may be collectively referred to as "structural units derived from 1,2- and 3,4-addition polymerization"). The remainder forms structural units polymerized via 1,4-bonds (hereinafter, these may be referred to as "structural units derived from 1,4-addition polymerization"). Of the structural units [b] derived from the linear conjugated diene compound in the block copolymer [C], the proportion of structural units derived from 1,2- and 3,4-addition polymerization is preferably 40% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, even more preferably 15% by mass or less, and still more preferably 10% by mass or less. When the proportion of structural units derived from 1,2- and 3,4-addition polymerization is not more than the above upper limit, the peak-top temperature of tan δ in the dynamic viscoelasticity of the resulting crosslinked elastomer composition can be easily adjusted to fall within the above-mentioned predetermined range. Furthermore, the lower limit of the proportion of structural units derived from 1,2- and 3,4-addition polymerization among the structural units [b] derived from a chain conjugated diene compound in the block copolymer [C] is not particularly limited, but may be 0% by mass or more, 1% by mass or more, 2% by mass or more, or 5% by mass or more. Note that the proportion of structural units derived from 1,2- and 3,4-addition polymerization among the structural units derived from a chain conjugated diene compound is 1 The ratio of the structural units [b] derived from a chain conjugated diene compound in the block copolymer [C] to the structural units derived from 1,2- and 3,4-addition polymerization can be controlled by, for example, the amount of a randomizer used in preparing the block copolymer [C].

[0044] [Method for Producing Block Copolymer [C]] The method for producing the block copolymer [C] is not particularly limited. For example, a method of alternately polymerizing a monomer mixture (a) containing an aromatic vinyl compound as a main component and a monomer mixture (b) containing a linear conjugated diene compound as a main component by a method such as living anionic polymerization; a method of sequentially polymerizing a monomer mixture (a) containing an aromatic vinyl compound as a main component and a monomer mixture (b) containing a linear conjugated diene compound as a main component, and then coupling the ends of the polymer block [B] with a coupling agent; etc. can be mentioned. Here, the monomer mixture (a) typically contains 95% by mass or more, preferably 98% by mass or more, of the aromatic vinyl compound relative to the entire mixture (a). Furthermore, the monomer mixture (b) typically contains 80% by mass or more, preferably 90% by mass or more, more preferably 95% by mass or more, of the linear conjugated diene compound relative to the entire mixture (b).

[0045] The coupling agent to be used is not particularly limited, and examples thereof include 1,2-dibromoethane, methyldichlorosilane, trichlorosilane, methyltrichlorosilane, tetrachlorosilane, tetramethoxysilane, divinylbenzene, diethyl adipate, dioctyl adipate, benzene-1,2,4-triisocyanate, tolylene diisocyanate, epoxidized 1,2-polybutadiene, epoxidized linseed oil, tetrachlorogermanium, tetrachlorotin, butyltrichlorotin, butyltrichlorosilane, dimethylchlorosilane, 1,4-chloromethylbenzene, and bis(trichlorosilyl)ethane.

[0046] During the preparation of the block copolymer [C] (particularly, polymerization for forming the polymer block [B]), the linear conjugated diene compound, and the aromatic vinyl compound and other vinyl compounds used as needed, can also be polymerized in the presence of a specific compound having an electron donor atom as a randomizer. As described above, the proportion of structural units derived from 1,2- and 3,4-addition polymerization among the structural units [b] derived from the linear conjugated diene compound in the resulting block copolymer [C] can be controlled by the amount of randomizer added.

[0047] The compound (randomizer) having an electron donor atom is preferably a compound having an electron donor atom such as oxygen (O) or nitrogen (N). Examples of the compound having an electron donor atom include ether compounds, amine compounds, and phosphine compounds.

[0048] Specific examples of compounds (randomizers) having an electron donor atom include diethyl ether, diisopropyl ether, dibutyl ether, tetrahydrofuran, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol diisopropyl ether, ethylene glycol dibutyl ether, ethylene glycol methylphenyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, propylene glycol diisopropyl ether, propylene glycol dibutyl ether, di(2-tetrahydrofuryl)methane, diethylene glycol dibutyl ether, dipropylene glycol dibutyl ether, tetramethylethylenediamine, etc. These may be used alone or in combination of two or more.

[0049] From the viewpoint of easily adjusting the ratio of the structural units derived from 1,2- and 3,4-addition polymerization, among the structural units [b] derived from a chain conjugated diene compound in the block copolymer [C], to fall within the above-mentioned predetermined range, the amount of the compound having an electron donor atom (randomizer) used is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and preferably 5.0 parts by mass or less, more preferably 2.0 parts by mass or less, relative to 100 parts by mass of the chain conjugated diene compound used.

[0050] [Hydrogenated Block Copolymer [D]] The hydrogenated block copolymer [D] is a polymer obtained by hydrogenating the carbon-carbon unsaturated bonds of the above-mentioned block copolymer [C]. Here, the carbon-carbon unsaturated bonds of the block copolymer [C] are not particularly limited and include carbon-carbon unsaturated bonds in the main chain and side chain derived from a linear conjugated diene compound and carbon-carbon unsaturated bonds in an aromatic ring derived from an aromatic vinyl compound.

[0051] The hydrogenation rate of the hydrogenated block copolymer [D] is preferably 95% or more, more preferably 97% or more, even more preferably 98% or more, and even more preferably 99% or more. When the hydrogenation rate of the hydrogenated block copolymer [D] is equal to or higher than the above-mentioned lower limit, the heat resistance of the crosslinked elastomer composition can be further improved. The upper limit of the hydrogenation rate of the hydrogenated block copolymer [D] is not particularly limited, and can be set to 100% or less. The hydrogenation rate of the hydrogenated block copolymer [D] can be measured using the method described in the Examples section of this specification.

[0052] The method for hydrogenating the block copolymer [C] is not particularly limited, and can be performed according to a known method. For example, when hydrogenating the carbon-carbon unsaturated bonds in the main chain and side chains derived from the linear conjugated diene compound in the block copolymer [C] and the carbon-carbon unsaturated bonds in the aromatic ring derived from the aromatic vinyl compound, for example, methods described in WO 2011 / 096389, WO 2012 / 043708, etc. can be used.

[0053] After completion of the hydrogenation reaction, the hydrogenation catalyst and / or polymerization catalyst can be removed from the reaction solution by a known method such as concentration and drying, and the hydrogenated block copolymer [D] can be recovered from the resulting solution. The temperature during concentration and drying can usually be 200° C. or higher and 300° C. or lower. The form of the recovered hydrogenated block copolymer [D] is not limited, but it can usually be made into pellets and then subjected to subsequent sheet forming or modification reactions.

[0054] The molecular weight of the hydrogenated block copolymer [D], as measured by GPC using THF as a solvent, is preferably 25,000 or more, more preferably 30,000 or more, even more preferably 35,000 or more, and preferably 200,000 or less, more preferably 170,000 or less, as a weight average molecular weight (Mw) calculated in terms of polystyrene. When the weight average molecular weight (Mw) of the hydrogenated block copolymer [D] is within the above-mentioned range, the heat resistance of the crosslinked elastomer composition can be further improved. Furthermore, the molecular weight distribution (Mw / Mn) of the hydrogenated block copolymer [D] is preferably 3.0 or less, more preferably 2.5 or less, and particularly preferably 2.0 or less. When the molecular weight distribution (Mw / Mn) of the hydrogenated block copolymer [D] is within the above-mentioned range, the heat resistance of the crosslinked elastomer composition can be further improved.

[0055] The hydrogenated block copolymer [D] preferably has a peak-top temperature of tan δ in the dynamic viscoelasticity measured in accordance with JIS K7244-2 of −70° C. or higher, more preferably −65° C. or higher, even more preferably −60° C. or higher, still more preferably −55° C. or higher, and preferably −35° C. or lower, more preferably −40° C. or lower, and even more preferably −45° C. or lower. When the peak-top temperature of tan δ in the dynamic viscoelasticity of the hydrogenated block copolymer [D] is within the above-mentioned range, an adhesive sheet obtained by molding the crosslinked elastomer composition can achieve both flexibility and heat resistance over a wide temperature range.

[0056] The peak top temperature of tan δ in the dynamic viscoelasticity of the hydrogenated block copolymer [D] and the value of tan δ at the peak top temperature are not particularly limited, but can be controlled, for example, by adjusting the proportion of structural units derived from a chain conjugated diene compound polymerized via 1,2-bonds and / or 3,4-bonds among structural units derived from a chain conjugated diene compound in the block copolymer [C] used in producing the hydrogenated block copolymer [D].

[0057] [Modified hydrogenated block copolymer [E]] The modified hydrogenated block copolymer [E] is obtained by introducing an alkoxysilyl group into the hydrogenated block copolymer [D] described above. By introducing an alkoxysilyl group into the hydrogenated block copolymer [D], it is possible to impart adhesion to inorganic materials such as glass, metals, etc. Furthermore, by introducing an alkoxysilyl group into the hydrogenated block copolymer [D], it is possible to make it easily crosslinkable in the presence of a condensation catalyst, which will be described later.

[0058] Examples of the alkoxysilyl group to be introduced include trialkoxysilyl groups such as trimethoxysilyl group, triethoxysilyl group, tripropoxysilyl group, etc.; alkyldialkoxysilyl groups such as methyldimethoxysilyl group, methyldiethoxysilyl group, ethyldimethoxysilyl group, ethyldiethoxysilyl group, propyldimethoxysilyl group, propyldiethoxysilyl group, etc.; dialkylalkoxysilyl groups such as dimethylmethoxysilyl group, dimethylethoxysilyl group, diethylmethoxysilyl group, diethylethoxysilyl group, dipropylmethoxysilyl group, dipropylethoxysilyl group, etc.; aryldialkoxysilyl groups such as phenyldimethoxysilyl group, phenyldiethoxysilyl group, etc. Among these, trialkoxysilyl groups and alkyldialkoxysilyl groups are preferred from the viewpoint of ease of availability of production raw materials, etc.

[0059] The alkoxysilyl group may be bonded directly to the hydrogenated block copolymer [D] or via a divalent organic group. Examples of the divalent organic group include alkylene groups having 1 to 10 carbon atoms, such as methylene, ethylene, propylene, and trimethylene; arylene groups having 6 to 20 carbon atoms, such as 1,4-phenylene and 1,4-naphthalene; ester groups, such as —C(═O)—O— and —O—C(═O)—; —C(═O)—; and combinations thereof.

[0060] The amount of the alkoxysilyl group introduced is usually 0.01 to 10 parts by mass, preferably 0.05 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, per 100 parts by mass of the hydrogenated block copolymer [D]. 1 The H-NMR spectrum (the number of integrations is increased when the amount introduced is small) is measured, and the adhesion coefficient can be calculated from the area ratio of the corresponding signals. If the amount of alkoxysilyl groups introduced is equal to or greater than the above-mentioned lower limit, even higher adhesiveness can be imparted. If the amount of alkoxysilyl groups introduced is equal to or less than the above-mentioned upper limit, crosslinking between alkoxysilyl groups due to trace amounts of moisture or the like can be suppressed during the process of introducing alkoxysilyl groups into the hydrogenated block copolymer [D] or during the storage period of the modified hydrogenated block copolymer [E] into which alkoxysilyl groups have been introduced, and sufficiently high moldability can be maintained.

[0061] The method for producing the modified hydrogenated block copolymer [E] by introducing an alkoxysilyl group into the hydrogenated block copolymer [D] is not particularly limited, and examples thereof include the methods described in WO 2012 / 043708 and JP 2015-78090 A.

[0062] A preferred method for producing the modified hydrogenated block copolymer [E] is to react the hydrogenated block copolymer [D] with an ethylenically unsaturated silane compound in the presence of an organic peroxide.

[0063] The ethylenically unsaturated silane compound to be used is not particularly limited as long as it can be graft polymerized with the hydrogenated block copolymer [D] and can introduce an alkoxysilyl group into the hydrogenated block copolymer [D]. For example, vinyltrialkoxysilanes such as vinyltrimethoxysilane and vinyltriethoxysilane; allyltrialkoxysilanes such as allyltrimethoxysilane and allyltriethoxysilane; dialkoxyalkylvinylsilanes such as dimethoxymethylvinylsilane and diethoxymethylvinylsilane; styryltrialkoxysilanes such as p-styryltrimethoxysilane and p-styryltriethoxysilane; ((meth)acryloxyalkyl)trialkoxysilanes such as 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-methacryloxypropyltriethoxysilane; ((meth)acryloxyalkyl)alkyldialkoxysilanes such as 3-methacryloxypropylmethyldimethoxysilane and 3-methacryloxypropylmethyldiethoxysilane; and the like. These ethylenically unsaturated silane compounds may be used either alone or in combination of two or more.

[0064] The amount of the ethylenically unsaturated silane compound used is usually 0.1 parts by mass or more and 10 parts by mass or less, preferably 0.5 parts by mass or more and 5 parts by mass or less, and more preferably 1 part by mass or more and 3 parts by mass or less, relative to 100 parts by mass of the hydrogenated block copolymer [D].

[0065] The peroxide preferably has a one-minute half-life temperature of 170 to 190°C. For example, t-butylcumyl peroxide, dicumyl peroxide, di-t-hexyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, di-t-butyl peroxide, di(2-t-butylperoxyisopropyl)benzene, etc. are preferably used. These peroxides may be used alone or in combination of two or more. The amount of peroxide used is usually 0.01 to 2 parts by mass, preferably 0.03 to 1 part by mass, and more preferably 0.05 to 0.5 parts by mass, per 100 parts by mass of the hydrogenated block copolymer [D].

[0066] The method for reacting the hydrogenated block copolymer [D] with the ethylenically unsaturated silane compound in the presence of a peroxide is not particularly limited. For example, alkoxysilyl groups can be introduced into the hydrogenated block copolymer [D] by kneading the mixture in a twin-screw kneader at a desired temperature for a desired time.

[0067] The kneading temperature in the twin-screw kneader is usually 180°C or higher and 240°C or lower, preferably 190°C or higher and 230°C or lower, and more preferably 200°C or higher and 220°C or lower. The heat kneading time is usually about 0.1 to 10 minutes, preferably 0.2 to 5 minutes, and more preferably 0.3 to 2 minutes. Continuous kneading and extrusion may be performed so that the temperature and residence time are within the above ranges. The form of the obtained modified hydrogenated block copolymer [E] is not limited, but it is usually made into pellets and can be subjected to subsequent molding processing, etc.

[0068] The molecular weight of the modified hydrogenated block copolymer [E], as measured by GPC using THF as a solvent, is preferably 20,000 or more, more preferably 25,000 or more, even more preferably 30,000 or more, particularly preferably 35,000 or more, and preferably 200,000 or less, more preferably 170,000 or less, as a weight average molecular weight (Mw) calculated in terms of polystyrene. When the weight average molecular weight (Mw) of the modified hydrogenated block copolymer [E] is within the above-mentioned range, the heat resistance of the crosslinked elastomer composition can be further improved. Furthermore, the molecular weight distribution (Mw / Mn) of the modified hydrogenated block copolymer [E] is preferably 4.0 or less, more preferably 3.5 or less, particularly preferably 3.0 or less. When the molecular weight distribution (Mw / Mn) of the modified hydrogenated block copolymer [E] is within the above-mentioned range, the heat resistance of the crosslinked elastomer composition can be further improved.

[0069] The peak top temperature of tan δ in the dynamic viscoelasticity of the modified hydrogenated block copolymer [E], measured in accordance with JIS K7244-2, is preferably −70° C. or higher, more preferably −65° C. or higher, even more preferably −60° C. or higher, still more preferably −55° C. or higher, and preferably −35° C. or lower, more preferably −40° C. or lower, and even more preferably −45° C. or lower. When the peak top temperature of tan δ in the dynamic viscoelasticity of the modified hydrogenated block copolymer [E] is within the above-mentioned range, an adhesive sheet obtained by molding the crosslinked elastomer composition can achieve both flexibility and heat resistance over a wide temperature range.

[0070] The peak top temperature of tan δ in the dynamic viscoelasticity of the modified hydrogenated block copolymer [E] and the value of tan δ at the peak top temperature are not particularly limited, but can be controlled, for example, by adjusting the proportion of structural units derived from a chain conjugated diene compound polymerized via 1,2-bonds and / or 3,4-bonds among structural units derived from a chain conjugated diene compound in the block copolymer [C] used in producing the modified hydrogenated block copolymer [E].

[0071] <<Crosslinking Method>> A crosslinked elastomer can be obtained by crosslinking a modified hydrogenated block copolymer such as the above-described modified hydrogenated block copolymer [E]. The method for crosslinking the modified hydrogenated block copolymer is not particularly limited, and any known crosslinking method can be used. Furthermore, since the above-described modified hydrogenated block copolymer has an alkoxysilyl group, which is a reactive group that undergoes a condensation reaction, it is preferable to use a method for crosslinking in the presence of a condensation catalyst.

[0072] Condensation catalysts used in crosslinking the modified hydrogenated block copolymer having alkoxysilyl groups include, for example, carboxylates (metal carboxylates) of metals such as calcium, barium, tin, zinc, iron, lead, and cobalt, organotitanium compounds, organozirconium compounds, organoaluminum compounds, organic bases, inorganic acids, and organic acids. More specifically, examples of the condensation catalyst include metal carboxylates such as calcium stearate, barium stearate, zinc stearate, zinc caprylate, dibutyltin dilaurate, dibutyltin dioleate, stannous octoate, and cobalt naphthenate; organic titanium compounds such as titanium(IV) acetylacetonate (also referred to as "tetrakis(2,4-pentanedionato)titanium(IV)"), tetrabutyl orthotitanate, tetranonyl orthotitanate, titanium-i-propoxyoctylene glycolate, diisopropylbis(acetylacetonyl)titanate, diisopropylbis(ethylacetoacetyl)titanate, and tetrabutyl titanate; and zirconium tetraacetylacetonate, zirconium Examples of suitable condensation catalysts include organic zirconium compounds such as tetraacetylacetonate, normal propyl zirconate, and normal butyl zirconate; organic aluminum compounds such as aluminum trisacetylacetonate, aluminum trisethylacetoacetate, and diisopropoxyaluminum ethylacetoacetate; organic bases such as dibutylamine, hexylamine, and pyridine; inorganic acids such as sulfuric acid and hydrochloric acid; and organic acids such as toluenesulfonic acid, acetic acid, stearic acid, maleic acid, and succinic acid. Among these, from the viewpoint of improving the adhesive properties and elongation of the adhesive sheet obtained by molding the crosslinked elastomer composition, it is preferable to use at least one of titanium (IV) acetylacetonate, maleic acid, and succinic acid as the condensation catalyst. These condensation catalysts may be used alone or in combination of two or more.

[0073] The amount of condensation catalyst used is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and preferably 5.00 parts by mass or less, more preferably 2.00 parts by mass or less, and even more preferably 1.00 parts by mass or less, per 100 parts by mass of the hydrogenated modified block copolymer used. If the amount of condensation catalyst used is above the above-mentioned lower limit, the heat resistance of the adhesive sheet obtained by molding the crosslinked elastomer composition can be further improved. On the other hand, if the amount of condensation catalyst used is below the above-mentioned upper limit, the elongation and adhesiveness of the adhesive sheet obtained by molding the crosslinked elastomer composition can be ensured to be sufficiently high.

[0074] Crosslinking of the modified hydrogenated block copolymer in the presence of a condensation catalyst can be carried out, for example, by the following method. A condensation catalyst is mixed with the modified hydrogenated block copolymer to obtain a resin composition. The obtained resin composition is melt-kneaded and uniformly mixed using a twin-screw kneader, extruder, or the like. The molten resin composition is then molded into a desired shape (e.g., a sheet). This allows the modified hydrogenated block copolymer to be crosslinked in the molten resin composition in the presence of the condensation catalyst, while obtaining a crosslinked elastomer composition containing the crosslinked elastomer as a molded product molded into a desired shape.

[0075] In the above, the temperature of the resin composition in a molten state is preferably 180°C or higher, more preferably 190°C or higher, and even more preferably 200°C or higher, and is preferably 240°C or lower, more preferably 230°C or lower, and even more preferably 220°C or lower. The heat-kneading time is usually about 0.1 to 10 minutes, preferably 0.2 to 7 minutes, and more preferably 0.3 to 5 minutes. Continuous kneading and extrusion may be performed so that the temperature and residence time are within the above ranges.

[0076] Here, the molded product obtained above (crosslinked elastomer composition containing a crosslinked elastomer) may be further subjected to a steam treatment in which the product is brought into contact with water vapor to further promote the crosslinking reaction. However, in the molded product obtained above, the crosslinking reaction has already progressed sufficiently, so it is preferable not to carry out the steam treatment from the viewpoint of production efficiency.

[0077] <Other Components> The crosslinked elastomer composition of the present invention may further contain components (other components) other than the crosslinked elastomer described above. The crosslinked elastomer composition of the present invention may further contain, as the other component, a condensation catalyst used in producing the crosslinked elastomer. Furthermore, the crosslinked elastomer composition of the present invention may further contain additives other than the crosslinked elastomer and the condensation catalyst, as long as the peak top temperature of tan δ in the dynamic viscoelasticity is within the above-mentioned predetermined range. As the additive, for example, the additives described in WO 2018 / 097146 can be used.

[0078] <Method for producing crosslinked elastomer composition> The method for producing the crosslinked elastomer composition of the present invention is not particularly limited, but preferably includes a crosslinking step of crosslinking the hydrogenated modified block copolymer in the presence of a condensation catalyst. The type and amount of the condensation catalyst used in the crosslinking step, and the method for crosslinking the hydrogenated modified block copolymer in the presence of a condensation catalyst can be the same as those described above in the section "Crosslinking method."

[0079] The crosslinked elastomer composition of the present invention can be suitably incorporated into an electrical and electronic sealing material. The shape of the electrical and electronic sealing material is not particularly limited, and in addition to the sheet form described below, any shape may be used as needed. When the electrical and electronic sealing material contains the crosslinked elastomer composition of the present invention, the electrical transmission sealing material exhibits excellent durability and can effectively protect the internal structure of the electrical and electronic devices to which it is applied from the external environment.

[0080] (Adhesive sheet and electrical / electronic sealing material comprising same) The adhesive sheet of the present invention is a sheet-like molded article obtained by molding the crosslinked elastomer composition of the present invention described above. The adhesive sheet of the present invention is obtained by molding the crosslinked elastomer composition of the present invention described above, and therefore has excellent heat resistance and solvent resistance. The adhesive sheet of the present invention is not particularly limited, but can be produced by melt-kneading a resin composition containing a modified hydrogenated block copolymer and a condensation catalyst using a twin-screw kneader or extruder, as in the method described above in the "Crosslinking method" section, and molding the resin composition into a sheet while crosslinking the modified hydrogenated block copolymer in the molten resin composition in the presence of the condensation catalyst. The thickness of the adhesive sheet is not particularly limited, and can be adjusted as appropriate depending on the application, etc.

[0081] Furthermore, the adhesive sheet of the present invention can be suitably used in the production of electrical and electronic encapsulants. In other words, the electrical and electronic encapsulants of the present invention suitably comprise the adhesive sheet of the present invention. By using the adhesive sheet of the present invention, particularly in the production of electrical and electronic encapsulants, the adhesive sheet exhibits particularly excellent durability and can effectively protect the internal structure of the applied electrical and electronic devices from the external environment.

[0082] (Laminated Glass) The laminated glass of the present invention is characterized by comprising the adhesive sheet of the present invention described above. Because the laminated glass of the present invention comprises the adhesive sheet of the present invention described above, it has excellent heat resistance and solvent resistance. The laminated glass of the present invention is, for example, formed by interposing at least one interlayer film between at least two glass plates and bonding them together, and the interlayer film comprises the adhesive sheet of the present invention described above. Here, the interlayer film may have a single-layer structure consisting of one adhesive sheet of the present invention, a multilayer structure consisting of two or more adhesive sheets of the present invention laminated together, or a multilayer structure consisting of one or more adhesive sheets of the present invention laminated together with one or more sheets other than the adhesive sheet of the present invention (other sheets). The other sheets are not particularly limited, but examples of the other sheets include the functional layers described in WO 2018 / 097146 and adhesive layers primarily composed of a thermoplastic resin. Furthermore, when the interlayer film comprises two or more adhesive sheets of the present invention, the compositions and thicknesses of the two or more adhesive sheets may be the same or different from each other.

[0083] The glass used in producing laminated glass is not particularly limited, and known inorganic glass such as float glass, polished glass, figured glass, wired glass, and heat-absorbing glass can be used. These glasses may be colorless or colored, transparent or opaque. They may be used alone or in combination of two or more. The shape of the glass is not particularly limited, and may be flat or curved. The material of the glass used is also not particularly limited. Examples include aluminosilicate glass, aluminoborosilicate glass, uranium glass, potassium glass, silicate glass, crystallized glass, germanium glass, quartz glass, soda glass, lead glass, barium lagosilicate glass, and lagosilicate glass.

[0084] The laminated glass of the present invention can be produced by a conventionally known method. For example, a method using a vacuum laminator, a method using a vacuum bag, a method using a vacuum ring, a method of pressurizing in an autoclave after temporary pressure bonding, etc. can be applied. When laminated glass is produced using thin, curved glass plates, the glass is very susceptible to breaking during the lamination process. Therefore, for example, a method such as that disclosed in JP 2016-36998 A can be used, in which a laminate formed by superposing a curved glass plate and an interlayer is placed in a polypropylene bag or the like, vacuum-packed, and temporarily pressure-bonded, and then pressurized and heated in an autoclave, thereby producing good laminated glass without breaking the glass.

[0085] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" representing amounts are based on mass unless otherwise specified. Various measurements and evaluations were performed according to the following methods.

[0086] (1) Measurement of Weight-Average Molecular Weight (Mw) and Molecular Weight Distribution (Mw / Mn) The molecular weights of the block copolymer [C1], the hydrogenated block copolymer [D1], and the modified hydrogenated block copolymer [E1] were measured at 38°C as values ​​converted into standard polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as an eluent. The measuring device used was a Tosoh HLC-8320GPC.

[0087] (2) Calculation of the proportion of structural units derived from 1,2- and 3,4-addition polymerization among structural units derived from a chain conjugated diene compound. 1 From the H-NMR spectrum (in deuterated chloroform), it was found that the carbon-carbon unsaturated bond in the polymer main chain 1 H bonded to the carbon of the carbon-carbon unsaturated bond in the polymer side chain 1 Based on the ratio of H, the proportions of structural units derived from 1,2- and 3,4-addition polymerization among the structural units derived from the chain conjugated diene compound were calculated.

[0088] (3) Measurement of hydrogenation rate The block copolymer [C1] and the hydrogenated block copolymer [D1] obtained by the hydrogenation reaction of the block copolymer [C1] were measured using deuterated chloroform as a solvent. 1 H-NMR measurement was carried out, and the proportion of lost unsaturated bonds among all unsaturated bonds present in the main chain, side chain, and aromatic ring of the block copolymer [C1] was calculated, thereby determining the hydrogenation rate of the hydrogenated block copolymer [D1].

[0089] (4) Measurement of Dynamic Viscoelasticity The pellets or sheet to be measured were placed in a 1 mm thick mold and pressed at 200°C for thermocompression bonding to produce a 1 mm thick sheet. A test piece measuring 50 mm in length and 10 mm in width was cut out from this sheet. Using this test piece, dynamic viscoelasticity was measured in accordance with JIS-K7244-2 using a viscoelasticity measuring device (manufactured by TA Instruments Japan, product name "ARES") at a frequency of 1 Hz, in the range of -100°C to +150°C, and at a heating rate of 5°C / min. The peak top temperature on the low-temperature side of the loss tangent tanδ and the value of tanδ at the peak top temperature were determined.

[0090] (5) Adhesion (Peel Strength) The pellets or sheets to be measured were placed in a 0.4 mm thick mold and thermocompressed at 200°C to produce a 0.4 mm thick sheet. A two-layer resin laminate sample for measuring peel strength was prepared from the sheet and a 1.0 mm thick aluminum plate. This sample was then cut to a size of 10 mm wide x 150 mm long to prepare a test piece for measuring peel strength. A portion of the interface between the resin sheet layer and the aluminum plate of this test piece was peeled off, and the test piece was fixed to a tensile tester (Shimadzu Corporation, product name "AGS-10kNX") so that only the resin sheet could be pulled. A 180° peel test was performed in accordance with JIS-K6854-2 at a peel rate of 50 mm / min to measure the peel strength.

[0091] (6) Elongation The pellets or sheets to be measured were placed in a 0.4 mm thick mold and pressed at 200°C for thermocompression bonding to produce a 0.4 m thick sheet. A JIS-K7127 type 5 1 / 2 size test piece was cut out from this sheet. Using this test piece, the breaking elongation was measured at a test speed of 50 mm / min using a tensile tester (manufactured by Shimadzu Corporation, product name "AGS-10kNX") based on the JIS-K7127 method.

[0092] (7) Heat Resistance Using the pellets or sheets to be measured, the offset method temperature was measured using a flow tester (manufactured by Shimadzu Corporation, product name "CFT-500EX") at an offset value of 1.0, a test force of 100, a temperature rise rate of 5°C / min, a die hole diameter of 1.0 mm, and a die length of 10 mm.

[0093] (8) Solvent Resistance 1.0 g of the pellets or sheets to be measured was added to a toluene solvent at room temperature (23°C) to a concentration of 1.0 mass%, and the mixture was stirred for 3 hours to dissolve. The solution was filtered using filter paper, and the filter paper was thoroughly dried to measure the mass of the remaining solid matter. The residual ratio was calculated from the mass.

[0094] Example 1 Production of Hydrogenated Block Copolymer [D1] 270 parts of dehydrated cyclohexane, 10 parts of dehydrated styrene, and 0.475 parts of dibutyl ether were placed in a reactor equipped with a stirrer and thoroughly purged with nitrogen. While stirring the entire contents at 60°C, 0.75 parts of n-butyllithium (15% cyclohexane solution) was added to initiate polymerization. Subsequently, while stirring the entire contents at 60°C, 15 parts of dehydrated styrene were continuously added to the reactor over 40 minutes to advance the polymerization reaction. After the addition was completed, the entire contents were stirred for an additional 20 minutes at 60°C. The resulting reaction solution was measured by gas chromatography (GC), and the polymerization conversion at this point was 99.5%. Next, 50 parts of dehydrated isoprene was continuously added to the reaction solution over 130 minutes, and stirring was continued for 30 minutes after the addition was completed. Analysis of the reaction solution at this point by GC revealed that the polymerization conversion was 99.5%. Thereafter, 25 parts of dehydrated styrene were continuously added to the reaction solution over 70 minutes, and after completion of the addition, the mixture was stirred for 60 minutes. At this point, the reaction solution was analyzed by GC, and the polymerization conversion rate was found to be nearly 100%. Next, 0.5 parts of isopropyl alcohol was added to terminate the reaction, yielding a polymer solution containing block copolymer [C1]. The weight-average molecular weight (Mw) of the block copolymer [C1] contained in the polymer solution was 43,000, the molecular weight distribution (Mw / Mn) was 1.08, wA:wB = 50:50, and the proportion of structural units derived from 1,2- and 3,4-addition polymerization was 8% of all structural units derived from isoprene. Next, the polymer solution was transferred to a pressure-resistant reactor equipped with a stirrer, and 7.0 parts of a diatomaceous earth-supported nickel catalyst (manufactured by JGC Catalysts and Chemicals, product name "E22U," nickel loading 60%) as a hydrogenation catalyst and 70 parts of dehydrated cyclohexane were added and mixed. The inside of the reactor was replaced with hydrogen gas, and hydrogen was further supplied to the solution while stirring, and the hydrogenation reaction was carried out at a temperature of 190° C. and a pressure of 4.5 MPa for 6 hours.After completion of the hydrogenation reaction, the reaction solution was filtered to remove the hydrogenation catalyst, and then 1.0 part of a xylene solution containing 0.1 part of pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (manufactured by Koyo Chemical Research Institute, product name "Songnox (registered trademark) 1010"), a phenolic antioxidant, was added to the filtrate and dissolved. Next, the solution was concentrated in a cylindrical concentrating dryer (manufactured by Hitachi, Ltd., CONTROL) at a temperature of 260°C and a pressure of 0.001 MPa or less to remove the solvents cyclohexane, xylene, and other volatile components from the solution. The molten polymer was continuously extruded through a die in the form of a strand, cooled, and then pelletized using a pelletizer to produce 93 parts of pellets of hydrogenated block copolymer [D1]. The resulting pellet-like hydrogenated block copolymer [D1] had a weight average molecular weight (Mw) of 42,700, a molecular weight distribution (Mw / Mn) of 1.50, and a hydrogenation rate of 99%.

[0095] <Production of Modified Hydrogenated Block Copolymer [E1]> 2.0 parts of vinyltrimethoxysilane, an ethylenically unsaturated silane compound, and 0.1 parts of 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, a peroxide (NOF Corporation, product name "Perhexa (registered trademark) 25B", temperature at which the half-life is 1 minute: 179.8°C), were added to 100 parts of pellets of the hydrogenated block copolymer [D1] and mixed in a blender. This mixture was continuously kneaded using a twin-screw extruder (Toshiba Machine Co., Ltd., TEM37B) at a resin temperature of 210°C and a residence time controlled to approximately 80 seconds. The kneaded resin was continuously extruded through a die attached to the twin-screw extruder at a die temperature of 210°C, formed into strands, and cooled to solidify. The solidified strand was cut using a pelletizer to produce 96 parts of pellets of the modified hydrogenated block copolymer [E1] having trimethoxysilyl groups. The IR spectrum of the surface of the produced pellets of the modified hydrogenated block copolymer [E1] was measured by the ATR method using an infrared spectrophotometer (iS5, manufactured by ThermoFisher Scientific). The IR spectrum included a peak at 1090 cm -1 Si-OCH 3 base, 825cm-1 and 739 cm -1 Si-CH 2 A new absorption band originating from the vinyltrimethoxysilane group was observed at 1075 cm -1 , 808 cm -1 , and 766 cm -1 The modified hydrogenated block copolymer [E1] pellets were observed at different positions. The weight average molecular weight (Mw) of the modified hydrogenated block copolymer [E1] pellets was 38,400, and the molecular weight distribution (Mw / Mn) was 2.37. 10 parts of the modified hydrogenated block copolymer [E1] pellets were dissolved in 100 parts of cyclohexane, and then the solution was poured into 400 parts of dehydrated methanol to coagulate the modified hydrogenated block copolymer [E1]. The coagulated product was collected by filtration and vacuum dried at 25°C to isolate 9.5 parts of crumbs of the modified hydrogenated block copolymer [E1]. 1 In the H-NMR spectrum (in deuterated chloroform), a peak due to the protons of the methoxy group was observed at 3.6 ppm, and from the peak area ratio, it was confirmed that 1.8 parts of vinyltrimethoxysilane were bonded to 100 parts of the hydrogenated block copolymer [D1].

[0096] <Production of Sheet [E1x] Made of Resin Composition Containing Crosslinked Elastomer> 1.0 parts of titanium (IV) acetylacetonate as a condensation catalyst was added to 100 parts of pellets of modified hydrogenated block copolymer [E1] and mixed to obtain a resin composition. The resulting resin composition was then crosslinked using a T-die film melt extrusion molding machine (T-die width 400 mm) equipped with a twin-screw kneader equipped with a 37 mmφ screw, and a sheet take-up device equipped with a cast roll (with embossed pattern) and a rubber nip roll, under conditions of a temperature of the molten resin composition of 210 ° C, a T-die temperature of 210 ° C, and a cast roll temperature of 40 ° C., to obtain a sheet [E1x] (thickness 0.20 mm) made of a crosslinked elastomer composition containing a crosslinked elastomer. The obtained sheet [E1x] was trimmed to a width of 330 mm using a slitter, and a release PET film (thickness 0.050 mm) was layered on top and wound into a roll for recovery. The peak top temperature of tan δ in the dynamic viscoelasticity of the obtained sheet [E1x] was −50° C., and the value of tan δ at the peak top temperature was 0.18. The obtained sheet [E1x] was used to evaluate the adhesiveness, elongation, heat resistance, and solvent resistance. The results are shown in Table 1.

[0097] Examples 2 and 3 Sheets [E1x] made of crosslinked elastomer compositions containing the hydrogenated block copolymer [D1], the hydrogenated modified block copolymer [E1], and the crosslinked elastomer were produced in the same manner as in Example 1, except that the type and / or amount of the condensation catalyst used in producing the sheet [E1x] made of the crosslinked elastomer composition containing the crosslinked elastomer was changed as shown in Table 1, and various measurements and evaluations were carried out. The results are shown in Table 1.

[0098] Comparative Example 1 Instead of producing sheet [E1x] made of a crosslinked elastomer composition containing a crosslinked elastomer, sheet [D1] made of a hydrogenated block copolymer was produced according to the following method, and the resulting sheet [D1] was used to evaluate adhesion, elongation, heat resistance, and solvent resistance. The results are shown in Table 2. <Production of Sheet [D1] Made of Hydrogenated Block Copolymer> 100 parts of pellets of the hydrogenated block copolymer [D1] produced in Example 1 were molded using a T-die type film melt extrusion molding machine (T-die width: 400 mm) equipped with a twin-screw kneader equipped with a 37 mmφ screw, and a sheet take-up device equipped with a cast roll (with an embossed pattern) and a rubber nip roll under conditions of a molten resin temperature of 210°C, a T-die temperature of 210°C, and a cast roll temperature of 40°C, to obtain sheet [D1] made of a hydrogenated block copolymer (thickness: 0.20 mm). The edge portions of the obtained sheet [D1] were cut off with a slitter to a width of 330 mm, and a release PET film (thickness 0.050 mm) was superimposed thereon, wound up into a roll, and collected. The peak top temperature of tan δ in the dynamic viscoelasticity of the obtained sheet [D1] was −49° C., and the value of tan δ at the peak top temperature was 0.18.

[0099] Comparative Example 2 A sheet [E1a] made of a modified hydrogenated block copolymer was produced according to the following method, and the resulting sheet [E1a] was used to evaluate adhesion, elongation, heat resistance, and solvent resistance. The results are shown in Table 2. <Production of Sheet [E1a] Made of Modified Hydrogenated Block Copolymer> 100 parts of pellets of the modified hydrogenated block copolymer [E1] produced in Example 1 were molded using a T-die film melt extrusion molding machine (T-die width: 400 mm) equipped with a twin-screw kneader equipped with a 37 mmφ screw, and a sheet take-up device equipped with a cast roll (with an embossed pattern) and a rubber nip roll under conditions of a molten resin temperature of 210°C, a T-die temperature of 210°C, and a cast roll temperature of 40°C, to obtain a sheet [E1a] made of a modified hydrogenated block copolymer (thickness: 0.20 mm). The edge portions of the obtained sheet [E1a] were cut off with a slitter to a width of 330 mm, and a release PET film (thickness 0.050 mm) was superimposed thereon, wound up into a roll, and collected. The peak top temperature of tan δ in the dynamic viscoelasticity of the obtained sheet [E1a] was −49°C, and the value of tan δ at the peak top temperature was 0.18.

[0100]

[0101]

[0102]

[0049] Table 1 shows that adhesive sheets with excellent heat resistance and solvent resistance can be formed using the crosslinked elastomer compositions of Examples 1 to 3, which contain a crosslinked elastomer obtained by crosslinking a modified hydrogenated block copolymer in which an alkoxysilyl group has been introduced to a hydrogenated block copolymer containing structural units derived from an aromatic vinyl compound and structural units derived from a linear conjugated diene compound, and which have a peak top temperature of tan δ in dynamic viscoelasticity within a specified range. On the other hand, in Comparative Example 1, in which an uncrosslinked hydrogenated block copolymer was used instead of the specified crosslinked elastomer composition, and in Comparative Example 2, in which an uncrosslinked hydrogenated modified block copolymer was used, the adhesive sheets formed were inferior in solvent resistance.

[0103] According to the present invention, a crosslinked elastomer composition capable of forming an adhesive sheet having excellent heat resistance and solvent resistance can be provided. Furthermore, according to the present invention, an adhesive sheet having excellent heat resistance and solvent resistance can be provided. Furthermore, according to the present invention, a laminated glass including the above adhesive sheet can be provided. Finally, according to the present invention, an electrical and electronic sealing material including the above crosslinked elastomer composition can be provided.

Claims

1. A crosslinked elastomer composition comprising a crosslinked elastomer obtained by crosslinking a modified hydrogenated block copolymer, wherein the modified hydrogenated block copolymer is a hydrogenated block copolymer containing a structural unit derived from an aromatic vinyl compound and a structural unit derived from a linear conjugated diene compound, to which an alkoxysilyl group has been introduced, and the crosslinked elastomer composition has a peak top temperature of tan δ in dynamic viscoelasticity measured in accordance with JIS K7244-2 of -70°C or higher and -35°C or lower.

2. The crosslinked elastomer composition according to claim 1, wherein the modified hydrogenated block copolymer is a hydrogenated block copolymer [D] obtained by hydrogenating carbon-carbon unsaturated bonds of a block copolymer [C] consisting of at least two polymer blocks [A] mainly composed of structural units derived from an aromatic vinyl compound and at least one polymer block [B] mainly composed of structural units derived from a chain-like conjugated diene compound, and an alkoxysilyl group is introduced into the hydrogenated block copolymer [D], wherein the mass fraction of all polymer blocks [A] in the block copolymer [C] in the entire block copolymer [C] is wA, and the mass fraction of all polymer blocks [B] in the block copolymer [C] in the entire block copolymer [C] is wB, and the ratio of wA to wB (wA:wB) is 30:70 to 60:

40.

3. The crosslinked elastomer composition according to claim 1, wherein the crosslinked elastomer is obtained by crosslinking the hydrogenated modified block copolymer in the presence of a condensation catalyst, and the condensation catalyst contains at least one selected from the group consisting of metal carboxylates, organotitanium compounds, organozirconium compounds, organoaluminum compounds, organic bases, inorganic acids, and organic acids.

4. The crosslinked elastomer composition according to any one of claims 1 to 3, wherein the condensation catalyst contains at least one of titanium (IV) acetylacetonate, maleic acid, and succinic acid.

5. A method for producing a crosslinked elastomer composition for producing the crosslinked elastomer composition according to claim 1, comprising a crosslinking step of crosslinking the hydrogenated modified block copolymer in the presence of a condensation catalyst, the condensation catalyst containing at least one selected from the group consisting of metal carboxylates, organotitanium compounds, organozirconium compounds, organoaluminum compounds, organic bases, inorganic acids, and organic acids.

6. The method for producing a crosslinked elastomer composition according to claim 5, wherein the condensation catalyst comprises at least one of titanium (IV) acetylacetonate, maleic acid, and succinic acid.

7. A method for producing a crosslinked elastomer composition according to claim 5 or 6, wherein the amount of the condensation catalyst used is 0.01 parts by mass or more and 5.00 parts by mass or less per 100 parts by mass of the hydrogenated modified block copolymer.

8. An adhesive sheet obtained by molding the crosslinked elastomer composition according to any one of claims 1 to 3.

9. A laminated glass comprising the adhesive sheet according to claim 8.

10. A sealing material for electrical and electronic devices, comprising the crosslinked elastomer composition according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Functional group-containing block copolymer and its composition

    JP2007314807A

  • Method of manufacturing molded body

    JP2014133848A

  • Methacrylic resin laminate and application thereof

    JP2021030668A

  • Adhesive sheet and laminated glass

    WO2018097146A1

  • Modified hydrogenated product, method for producing same, resin composition, and various uses thereof

    WO2019230527A1