Photocurable composition for adhesive sheet, adhesive sheet, optical laminate, and image display device
The photocurable composition with a specific photopolymerization initiator structure addresses the balance between polymerization rate and residual content in adhesive sheets, enhancing performance by achieving high polymerization efficiency with minimal residual initiator, thus reducing defects like yellowing and foaming.
Patent Information
- Application Number
- PCT/JP2024/009902
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-13
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional photocurable adhesive sheets face challenges in achieving a balance between polymerization rate and residual photopolymerization initiator content, leading to issues like yellowing and foaming, with insufficient consideration given to both factors in existing compositions.
A photocurable composition incorporating a specific photopolymerization initiator with a defined chemical structure, which improves polymerization rate and reduces the residual amount of the initiator, is used to form pressure-sensitive adhesive sheets.
The composition achieves a high polymerization rate of 96% or more while maintaining a low residual photopolymerization initiator content of 800 wtppm or less, thereby minimizing issues like yellowing and foaming and ensuring consistent adhesive performance.
Smart Images

Figure JP2024009902_03102024_PF_FP_ABST
Abstract
Description
Photocurable composition for pressure-sensitive adhesive sheet, pressure-sensitive adhesive sheet, optical laminate, and image display device
[0001] The present invention relates to a photocurable composition for a pressure-sensitive adhesive sheet, a pressure-sensitive adhesive sheet, an optical laminate, and an image display device.
[0002] Various image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices, generally include an optical laminate including an optical film such as a polarizing film and an adhesive sheet. An adhesive sheet is typically used to bond the optical films included in the optical laminate or to bond the optical laminate to an image display panel. A typical adhesive sheet is a sheet formed by polymerizing and crosslinking a group of monomers, including acrylic monomers and silicone monomers. Patent Document 1 discloses an adhesive sheet formed from a photocurable composition (hereinafter referred to as a photocurable adhesive sheet). Another type of adhesive sheet is an adhesive sheet formed by thermally curing a layer containing an adhesive composition and a solvent (hereinafter referred to as a thermosetting adhesive sheet).
[0003] Japanese Patent Application Laid-Open No. 2019-70150
[0004] Photocurable adhesive sheets tend to have more residual monomers than thermosetting adhesive sheets. Residual monomers can generate odors. To reduce the residual amount, it is conceivable to increase the amount of photopolymerization initiator blended to improve the polymerization rate. However, according to the inventors' studies, simply increasing the blended amount increases the amount of photopolymerization initiator remaining in the adhesive sheet, which can lead to other problems such as yellowing and foaming. Conventionally, photocurable compositions for forming adhesive sheets have not been sufficiently designed to take into account both the polymerization rate and the amount of residual photopolymerization initiator.
[0005] An object of the present invention is to provide a photocurable composition suitable for improving the polymerization rate and reducing the amount of residual photopolymerization initiator when forming a pressure-sensitive adhesive sheet.
[0006] The present invention provides a photocurable composition for a pressure-sensitive adhesive sheet, comprising a group of monomers and / or a partial polymer of the group of monomers, and a photopolymerization initiator, wherein the photopolymerization initiator is a compound having a chemical structure represented by the following formula (1) in its molecule, and R in the formula (1)1 and R 2 are each independently a C1 to C8 alkyl group; —OH, a C1 to C4 alkoxy group, —CN, —COOR 51 , -OOCR 52 , or -NR 53 R 54 a C1-C4 alkyl group in which a hydrogen atom is substituted by -; a C3-C6 alkenyl group; or -CH2-C6H4-R 55 and R 1 and R 2 may be bonded to each other to form a C2 to C9 alkylene group, or a C3 to C6 oxyalkylene group or an azaalkylene group, and X is -OR 56 , or -NR 57 R 58 and R 51 is a C1 to C8 alkyl group, R 52 is a C1-C4 alkyl group, R 53 and R 54 are each independently a hydrogen atom, a C1 to C12 alkyl group; —OH, a C1 to C4 alkoxy group, —CN, or —COOR 59 a C2-C4 alkyl group in which a hydrogen atom is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group; 53 and R 54 are bonded to each other to form —O— or —N(R 60 )-, and R may be a C3 to C9 alkylene group optionally interrupted by -. 55 is a C1-C4 alkyl group, R 56 is a hydrogen atom, -SiR 62 3. A C1-C8 alkyl group or a C3-C6 alkenyl group, R 57 and R 58 represents a C1 to C12 alkyl group; —OH, a C1 to C4 alkoxy group, —CN, and —COOR 63 a C2-C4 alkyl group in which a hydrogen atom is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group; 57and R 58 are bonded to each other to form —O— or —N(R 64 )-, and R may be a C3 to C9 alkylene group optionally interrupted by -. 59 is a C1-C4 alkyl group, R 60 represents a hydrogen atom, a C1-C4 alkyl group, an allyl group, a C1-C4 hydroxyalkyl group, -CH2CH2-COOR 61 or —CH2CH2CN, R 61 is a C1-C4 alkyl group, R 62 is a C1 to C6 alkyl group, R 63 is a C1-C4 alkyl group, R 64 represents a hydrogen atom, a C1-C4 alkyl group, an allyl group, a C1-C4 hydroxyalkyl group, -CH2CH2-COOR 65 or —CH2CH2CN, R 65 is a C1 to C4 alkyl group, and the chemical structure can be bonded to a hydrogen atom or a hydrogen atom-substituted structure via the carbon atom indicated by * in formula (1).
[0007]
[0008] The present invention further provides a pressure-sensitive adhesive sheet formed from the above photocurable composition.
[0009] The present invention further provides an optical laminate comprising the above pressure-sensitive adhesive sheet and an optical film.
[0010] The present invention further provides an image display device comprising the above optical laminate.
[0011] According to the present invention, it is possible to provide a photocurable composition suitable for improving the polymerization rate and reducing the amount of residual photopolymerization initiator when forming a pressure-sensitive adhesive sheet.
[0012] FIG. 1 is a cross-sectional view schematically showing an example of a pressure-sensitive adhesive sheet of the present invention. FIG. 2 is a schematic view for explaining an example of a method for forming the pressure-sensitive adhesive sheet of the present invention from the photocurable composition of the present invention. FIG. 3 is a cross-sectional view schematically showing an example of an optical laminate of the present invention. FIG. 4 is a cross-sectional view schematically showing an example of an optical laminate of the present invention. FIG. 5 is a cross-sectional view schematically showing an example of an optical laminate of the present invention. FIG. 6 is a cross-sectional view schematically showing an example of an image display device of the present invention. FIG. 7 is a graph showing the relationship between the polymerization rate and the content of a photopolymerization initiator in the pressure-sensitive adhesive sheets of Examples and Comparative Examples.
[0013] A photocurable composition according to a first aspect of the present invention is a photocurable composition for pressure-sensitive adhesive sheets, comprising a group of monomers and / or a partial polymer of the group of monomers, and a photopolymerization initiator, wherein the photopolymerization initiator is a compound having a chemical structure represented by the following formula (1) in its molecule, and R in the formula (1) 1 and R 2 are each independently a C1 to C8 alkyl group; —OH, a C1 to C4 alkoxy group, —CN, —COOR 51 , -OOCR 52 , or -NR 53 R 54 a C1-C4 alkyl group in which a hydrogen atom is substituted by -; a C3-C6 alkenyl group; or -CH2-C6H4-R 55 and R 1 and R 2 may be bonded to each other to form a C2 to C9 alkylene group, or a C3 to C6 oxyalkylene group or an azaalkylene group, and X is -OR 56 , or -NR 57 R 58 and R 51 is a C1 to C8 alkyl group, R 52 is a C1-C4 alkyl group, R 53 and R 54 are each independently a hydrogen atom, a C1 to C12 alkyl group; —OH, a C1 to C4 alkoxy group, —CN, or —COOR 59a C2-C4 alkyl group in which a hydrogen atom is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group; 53 and R 54 are bonded to each other to form —O— or —N(R 60 )-, and R may be a C3 to C9 alkylene group optionally interrupted by -. 55 is a C1-C4 alkyl group, R 56 is a hydrogen atom, -SiR 62 3. A C1-C8 alkyl group or a C3-C6 alkenyl group, R 57 and R 58 represents a C1 to C12 alkyl group; —OH, a C1 to C4 alkoxy group, —CN, and —COOR 63 a C2-C4 alkyl group in which a hydrogen atom is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group; 57 and R 58 are bonded to each other to form —O— or —N(R 64 )-, and R may be a C3 to C9 alkylene group optionally interrupted by -. 59 is a C1-C4 alkyl group, R 60 represents a hydrogen atom, a C1-C4 alkyl group, an allyl group, a C1-C4 hydroxyalkyl group, -CH2CH2-COOR 61 or —CH2CH2CN, R 61 is a C1-C4 alkyl group, R 62 is a C1 to C6 alkyl group, R 63 is a C1-C4 alkyl group, R 64 represents a hydrogen atom, a C1-C4 alkyl group, an allyl group, a C1-C4 hydroxyalkyl group, -CH2CH2-COOR 65 or —CH2CH2CN, R 65 is a C1 to C4 alkyl group, and the chemical structure can be bonded to a hydrogen atom or a hydrogen atom-substituted structure via the carbon atom marked with * in formula (1).
[0014] In the second aspect of the present invention, for example, in the photocurable composition according to the first aspect, the R 1 and the R 2 are each independently a C1 to C8 alkyl group.
[0015] In the third aspect of the present invention, for example, in the photocurable composition according to the first or second aspect, the R 1 and the R 2 are identical.
[0016] In a fourth aspect of the present invention, for example, in the photocurable composition according to any one of the first to third aspects, X is -OR 56 is.
[0017] In a fifth aspect of the present invention, for example, in the photocurable composition according to any one of the first to third aspects, X is —OH.
[0018] In a sixth aspect of the present invention, for example, in the photocurable composition according to any one of the first to fifth aspects, the chemical structure is a structure represented by the following formula (2).
[0019] In a seventh aspect of the present invention, for example, in the photocurable composition according to any one of the first to sixth aspects, the photopolymerization initiator is a compound having two or more of the chemical structures in one molecule.
[0020] In an eighth aspect of the present invention, for example, in the photocurable composition according to any one of the first to seventh aspects, the photopolymerization initiator is a compound represented by the following formula (3), and R in the formula (3) 1 ' and R 2 ' are each other and the R 1 and R 2 Independently of R 1 and R 2 X' is, independently of X, a group that can be taken as X; A is -O-, -CYR 3 - or -C(CH3)R 4 Y is a hydrogen atom, —Cl, —Br, —O—R 71 , -NR 72 R73 , or -S-R 74 and R 3 represents a hydrogen atom, a C1-C8 alkyl group, a C3-C6 alkenyl group, a benzyl group, -CH2-C6H4-R 75 or a phenyl group, R 4 is a C1 to C6 alkyl or alkylene group, and the alkylene group is bonded to a carbon atom of the phenylene group of the compound of formula (3), and R 71 is a hydrogen atom, -Si(R 76 ) 3, C1 to C12 alkyl group, C2 to C18 acyl group, —CO—NH—R 77 , a C2 to C20 hydroxyalkyl group, a C2 to C20 methoxyalkyl group, 3-R 78 -2-hydroxypropyl group, 3-[1,3,3,3-tetramethyl-1-[(trimethylsilyl)oxy]disiloxanyl]propyl group, 2,3-dihydroxypropyl group, or a C2-C21 hydroxyalkyl group or a C3-C25 alkyl group in which the carbon chain is interrupted by 1 to 9 oxygen atoms, R 72 and R 73 are each independently a C1 to C12 alkyl group; —OH, a C1 to C4 alkoxy group, —CN, and —COOR 79 a C2-C4 alkyl group in which a hydrogen atom is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; a cyclohexyl group; or a C7-C9 phenylalkyl group, 72 and R 73 are bonded to each other to form —O— or —N(R 80 )-, and R may be a C3 to C9 alkylene group optionally interrupted by -. 74 represents a C1 to C18 alkyl group, a hydroxyethyl group, a 2,3-dihydroxypropyl group, a cyclohexyl group, a benzyl group, a phenyl group, a C1 to C12 alkylphenyl group, -CH2-COOR 81 -CH2CH2-COOR 82 , or —CH(CH3)—COOR 83 And R 75 is a C1-C4 alkyl group, R76 is a C1 to C6 alkyl group, R 77 is a C1 to C12 alkyl group, R 78 is a C1 to C18 alkoxy group, R 79 is a C1-C4 alkyl group, R 80 represents a hydrogen atom, a C1-C4 alkyl group, an allyl group, a benzyl group, a C1-C4 hydroxyalkyl group, -CH2CH2-COOR 84 or —CHCHCN, R 81 , R 82 and R 83 are each independently a C1 to C18 alkyl group, R 84 is a C1 to C4 alkyl group.
[0021] In a ninth aspect of the present invention, for example, in the photocurable composition according to the eighth aspect, A is -CYR 3 - is.
[0022] In a tenth aspect of the present invention, for example, in the photocurable composition according to the ninth aspect, the Y and R 3 is a hydrogen atom.
[0023] In an eleventh aspect of the present invention, for example, in the photocurable composition according to any one of the eighth to tenth aspects, the photopolymerization initiator is a compound represented by the following formula (4):
[0024] In a twelfth aspect of the present invention, for example, in the photocurable composition according to any one of the first to eleventh aspects, the amount of the photopolymerization initiator in the photocurable composition is 0.01 to 1 part by weight per 100 parts by weight of the total of the monomer group and the partially polymerized product.
[0025] In a thirteenth aspect of the present invention, for example, in the photocurable composition according to any one of the first to twelfth aspects, the group of monomers includes a (meth)acrylic monomer.
[0026] A pressure-sensitive adhesive sheet according to a fourteenth aspect of the present invention is a pressure-sensitive adhesive sheet formed from the photocurable composition according to any one of the first to thirteenth aspects.
[0027] In a fifteenth aspect of the present invention, for example, in the pressure-sensitive adhesive sheet according to the fourteenth aspect, the polymerization rate of the monomer group in the pressure-sensitive adhesive sheet is 96% or more, and the content of the photopolymerization initiator is 800 wtppm or less.
[0028] In a sixteenth aspect of the present invention, for example, in the pressure-sensitive adhesive sheet according to the fourteenth or fifteenth aspect, the thickness of the pressure-sensitive adhesive sheet is 300 μm or less.
[0029] An optical laminate according to a seventeenth aspect of the present invention comprises the pressure-sensitive adhesive sheet according to any one of the fourteenth to sixteenth aspects and an optical film.
[0030] In an eighteenth aspect of the present invention, for example, in the optical laminate according to the seventeenth aspect, the optical film is a polarizing film, and the pressure-sensitive adhesive sheet is in contact with the polarizing film.
[0031] An image display device according to a nineteenth aspect of the present invention includes the optical laminate according to the seventeenth or eighteenth aspect.
[0032] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be implemented in any modified form within the scope of the gist of the present invention.
[0033] [Photocurable composition] The photocurable composition of this embodiment contains a monomer group and / or a partial polymer of the monomer group, and a photopolymerization initiator. The photocurable composition of this embodiment is for use in a pressure-sensitive adhesive sheet. A pressure-sensitive adhesive sheet can be formed from the photocurable composition of this embodiment.
[0034] (Photopolymerization Initiator) The photopolymerization initiator contained in the photocurable composition of this embodiment is a compound having a chemical structure represented by the following formula (1) in the molecule (hereinafter referred to as chemical structure X).
[0035] R in the formula (1) 1 and R 2 are each independently a C1 to C8 alkyl group; —OH, a C1 to C4 alkoxy group, —CN, —COOR 51 , -OOCR 52 , or -NR53 R 54 a C1-C4 alkyl group in which a hydrogen atom is substituted by -; a C3-C6 alkenyl group; or -CH2-C6H4-R 55 It is. 1 and R 2 may be bonded to each other to form a C2 to C9 alkylene group, a C3 to C6 oxyalkylene group, or an azaalkylene group. 51 is a C1 to C8 alkyl group. 52 is a C1 to C4 alkyl group. 53 and R 54 are each independently a hydrogen atom, a C1 to C12 alkyl group; —OH, a C1 to C4 alkoxy group, —CN, or —COOR 59 a C2-C4 alkyl group in which a hydrogen atom is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group. 53 and R 54 are bonded to each other to form —O— or —N(R 60 )-Optionally, it may be a C3 to C9 alkylene group. 55 is a C1 to C4 alkyl group. 59 is a C1 to C4 alkyl group. 60 represents a hydrogen atom, a C1-C4 alkyl group, an allyl group, a C1-C4 hydroxyalkyl group, -CH2CH2-COOR 61 Or -CH2CH2CN. 61 is a C1 to C4 alkyl group.
[0036] X is -OR 56 , or -NR 57 R 58 It is. 56 is a hydrogen atom, -SiR 62 3. A C1 to C8 alkyl group or a C3 to C6 alkenyl group. 57 and R 58 represents a C1 to C12 alkyl group; —OH, a C1 to C4 alkoxy group, —CN, and —COOR 63a C2-C4 alkyl group in which a hydrogen atom is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group. 57 and R 58 are bonded to each other to form —O— or —N(R 64 )-Optionally, it may be a C3 to C9 alkylene group. 62 is a C1 to C6 alkyl group. 63 is a C1 to C4 alkyl group. 64 represents a hydrogen atom, a C1-C4 alkyl group, an allyl group, a C1-C4 hydroxyalkyl group, -CH2CH2-COOR 65 Or -CH2CH2CN. 65 is a C1 to C4 alkyl group.
[0037] The chemical structure X can be bonded to a hydrogen atom or a structure substituted with a hydrogen atom through the carbon atom indicated by * in formula (1).
[0038] The alkyl group, alkoxy group, alkenyl group, alkylene group, oxyalkylene group, azaalkylene group, and hydroxyalkyl group described in the explanation of formula (1) may be unbranched or branched. Furthermore, the expression "Cn1 to Cn2" (n1 and n2 are natural numbers) in this specification, including the explanation of formula (1), means that the number of carbon atoms is in the range of n1 to n2.
[0039] According to the investigations of the present inventors, chemical structure X is suitable for suppressing inhibition by oxygen during photocuring of the photocurable composition, which is thought to contribute to improving the cleavage efficiency of the photopolymerization initiator.
[0040] R 1 and R 2 may be, independently of each other, a C1 to C8 alkyl group, a C3 to C6 alkenyl group, or a C1 to C8 alkyl group. 1 and R 2 may be, independently of each other, a C1 to C4 alkyl group, a C1 to C3 alkyl group, or a C1 to C2 alkyl group. 1 and R2 may be a methyl group.
[0041] R 1 and R 2 may be the same.
[0042] X is -OR 56 R 56 may be a hydrogen atom or a C1 to C8 alkyl group, or may be a hydrogen atom. In other words, X may be —OH.
[0043] R 1 , R 2 and X may take any combination of the above preferred examples.
[0044] The chemical structure X may be a structure shown in the following formula (2): In the chemical structure X of formula (2), when a substitution structure of a hydrogen atom is bonded to the carbon atom indicated by *, the substitution structure and —COCR in formula (2) 1 XR 2 The group is in a para-position relationship with respect to the benzene ring of the chemical structure X.
[0045] The photopolymerization initiator may be a compound having two or more chemical structures X in one molecule. A photopolymerization initiator having two or more chemical structures X in one molecule can reliably contribute to both the formation of a polymer from a monomer and the extension of a polymer chain when incorporated into a polymer. This photopolymerization initiator is particularly suitable for improving the polymerization rate and reducing the amount of residual photopolymerization initiator when forming a pressure-sensitive adhesive sheet.
[0046] The photopolymerization initiator may be a compound represented by the following formula (3). The compound of formula (3) has two chemical structures X in one molecule. The two chemical structures X are located at both ends of the photopolymerization initiator molecule. More specifically, the two chemical structures X are bonded to each other via -A- at the carbon atom of the phenylene group represented by * above.
[0047] R in formula (3) 1 ' and R 2 ' are mutually exclusive and R 1 and R 2 Independently of1 and R 2 R 1 ' and / or R 2 ' is R 1 and / or R 2 may be the same as R 1 , R 2 , R 1 ' and R 2 ' may all be the same.
[0048] X' in formula (3) is a group that can be taken as X, independently of X in formula (1). X' and X may be the same.
[0049] A is -O-, -CYR 3 - or -C(CH3)R 4 is.
[0050] Y is a hydrogen atom, —Cl, —Br, or —O—R 71 , -NR 72 R 73 , or -S-R 74 It is. 3 represents a hydrogen atom, a C1-C8 alkyl group, a C3-C6 alkenyl group, a benzyl group, -CH2-C6H4-R 75 or a phenyl group. 4 is a C1-C6 alkyl or alkylene group, and this alkylene group is bonded to a carbon atom of the phenylene group of the compound of formula (3).
[0051] R 71 is a hydrogen atom, -Si(R 76 ) 3, C1 to C12 alkyl group, C2 to C18 acyl group, —CO—NH—R 77 , a C2 to C20 hydroxyalkyl group, a C2 to C20 methoxyalkyl group, 3-R 78 -2-hydroxypropyl group, 3-[1,3,3,3-tetramethyl-1-[(trimethylsilyl)oxy]disiloxanyl]propyl group, 2,3-dihydroxypropyl group, or a C2 to C21 hydroxyalkyl group or a C3 to C25 alkyl group in which the carbon chain is interrupted by 1 to 9 oxygen atoms. 72 and R 73are each independently a C1 to C12 alkyl group; —OH, a C1 to C4 alkoxy group, —CN, and —COOR 79 a C2-C4 alkyl group in which a hydrogen atom is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; a cyclohexyl group; or a C7-C9 phenylalkyl group. 72 and R 73 are bonded to each other to form —O— or —N(R 80 )-Optionally, it may be a C3 to C9 alkylene group. 74 represents a C1 to C18 alkyl group, a hydroxyethyl group, a 2,3-dihydroxypropyl group, a cyclohexyl group, a benzyl group, a phenyl group, a C1 to C12 alkylphenyl group, -CH2-COOR 81 -CH2CH2-COOR 82 , or —CH(CH3)—COOR 83 It is. 75 is a C1 to C4 alkyl group. 76 is a C1 to C6 alkyl group. 77 is a C1 to C12 alkyl group. 78 is a C1 to C18 alkoxy group. 79 is a C1 to C4 alkyl group. 80 represents a hydrogen atom, a C1-C4 alkyl group, an allyl group, a benzyl group, a C1-C4 hydroxyalkyl group, -CH2CH2-COOR 84 , or —CH2CH2CN. 81 , R 82 and R 83 are each independently a C1 to C18 alkyl group. 84 is a C1 to C4 alkyl group.
[0052] The alkyl group, alkenyl group, acyl group, hydroxyalkyl group, methoxyalkyl group, alkoxy group, alkyl moiety in the phenylalkyl group, and alkylene group described in the explanation of formula (3) may all be unbranched or branched.
[0053] R in formula (3) 1 , R 2, R 1 ' and R 2 Preferred examples of R ′ are those described above in the explanation of formula (1). 1 and R 2 The preferred examples of X′ in formula (3) are the same as the preferred examples of X described above in the explanation of formula (1). A is —CYR 3 -. Y may be a hydrogen atom. R 3 may be a hydrogen atom. 3 - and Y and R 3 and may both be hydrogen atoms. In other words, A may be —CH—.
[0054] R in formula (3) 1 , R 2 , R 1 ', R 2 ', X, X', and A may take any combination of the preferred examples above.
[0055] The photopolymerization initiator may be a compound represented by the following formula (4): The compound of formula (4) is a type of compound of formula (3).
[0056] Specific examples of photopolymerization initiators are shown in the following formulas (5) to (9). The photopolymerization initiator may be a compound represented by at least one formula selected from the group consisting of formulas (5) to (9), a compound represented by at least one formula selected from the group consisting of formulas (5) to (8), a compound represented by at least one formula selected from the group consisting of formulas (5) to (7), or a compound represented by formula (5). The compound of formula (8) is derived from a vinyl compound having chemical structure X in its side chain. More specifically, it is an oligomer of the vinyl compound.
[0057]
[0058]
[0059]
[0060]
[0061]
[0062] The photopolymerization initiators represented by formulas (5) to (9) are commercially available as Omnirad 127, Esacure KIP 160, Esacure one, Esacure KIP 150, and Omnirad 1173 (all manufactured by IGM Resins). The photopolymerization initiator may be at least one selected from these groups.
[0063] The photocurable composition may include one or more photoinitiators.
[0064] The amount of the photopolymerization initiator in the photocurable composition is, for example, 0.01 to 1 part by weight per 100 parts by weight of the total of the monomer group and the partially polymerized product. When two or more photopolymerization initiators are included, the total amount of each photopolymerization initiator falls within this range. The upper limit of the amount may be 0.9 parts by weight or less, 0.8 parts by weight or less, 0.7 parts by weight or less, 0.6 parts by weight or less, 0.5 parts by weight or less, 0.4 parts by weight or less, 0.3 parts by weight or less, 0.25 parts by weight or less, 0.22 parts by weight or less, or even 0.2 parts by weight or less. The lower limit of the amount may be 0.05 parts by weight or more, 0.08 parts by weight or more, 0.1 parts by weight or more, or even 0.15 parts by weight or more.
[0065] (Monomer Group) The monomer group may contain a (meth)acrylic monomer. The content of the (meth)acrylic component, i.e., the (meth)acrylic monomer and its partial polymer, in the photocurable composition may be 50% by weight or more, 60% by weight or more, 70% by weight or more, or even 80% by weight or more. In this case, an acrylic pressure-sensitive adhesive sheet containing a (meth)acrylic polymer and its crosslinked product as the main components can be formed. However, the photocurable composition is not limited to the above examples. In this specification, (meth)acrylic means acrylic and methacrylic. (Meth)acrylate means acrylate and methacrylate.
[0066] An example of the (meth)acrylic monomer is a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 20 carbon atoms on the side chain. The number of carbon atoms in the alkyl group may be 7 or less, 6 or less, 5 or less, or even 4 or less. The alkyl group may be linear or branched. Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. acrylate, n-octyl(meth)acrylate, isooctyl(meth)acrylate, n-nonyl(meth)acrylate, isononyl(meth)acrylate, n-decyl(meth)acrylate, isodecyl(meth)acrylate, n-dodecyl(meth)acrylate (lauryl(meth)acrylate), n-tridecyl(meth)acrylate, n-tetradecyl(meth)acrylate, pentadecyl(meth)acrylate, hexadecyl(meth)acrylate, heptadecyl(meth)acrylate, and octadecyl(meth)acrylate. The (meth)acrylic acid alkyl ester may be n-butyl(meth)acrylate.
[0067] The content of the (meth)acrylic acid alkyl ester in the monomer group is, for example, 40% by weight or more, and may be 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, or even 95% by weight or more. In calculating the content, the weight of the partially polymerized product is converted into the weight of each monomer before polymerization.
[0068] The monomer group may contain a carboxyl group-containing monomer. The carboxyl group-containing monomer may be a (meth)acrylic monomer; in other words, the (meth)acrylic monomer may contain a carboxyl group-containing monomer. Examples of carboxyl group-containing monomers include (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid. The content of the carboxyl group-containing monomer in the monomer group may be, for example, 10% by weight or less, 9% by weight or less, 8% by weight or less, 7% by weight or less, 6% by weight or less, 5.5% by weight or less, or even 5% by weight or less. The lower limit of the content may be, for example, 0.1% by weight or more, 0.5% by weight or more, or even 1% by weight or more. The monomer group may not contain a carboxyl group-containing monomer.
[0069] The monomer group may contain a hydroxy group-containing monomer. The hydroxy group-containing monomer may be a (meth)acrylic monomer, in other words, the (meth)acrylic monomer may contain a hydroxy group-containing monomer. The hydroxy group-containing monomer may contribute to improving the cohesive strength of the PSA sheet. Examples of hydroxy group-containing monomers are 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)-methyl acrylate. The hydroxy group-containing monomer is preferably 2-hydroxyethyl (meth)acrylate or 4-hydroxybutyl (meth)acrylate. The content of the hydroxy group-containing monomer in the monomer group is, for example, 10% by weight or less, and may be 5% by weight or less, 4% by weight or less, 3% by weight or less, 2% by weight or less, 1% by weight or less, 0.8% by weight or less, 0.5% by weight or less, 0.3% by weight or less, 0.2% by weight or less, or even 0.1% by weight or less. The lower limit of the content may be, for example, 0.01% by weight or more, 0.03% by weight or more, or even 0.05% by weight or more. The monomer group may not contain a hydroxy group-containing monomer.
[0070] The monomer group may include a nitrogen atom-containing monomer. The nitrogen atom-containing monomer means a monomer having at least one nitrogen atom in the molecule (per molecule).
[0071] As the nitrogen atom-containing monomer, from the viewpoint of improving foaming and peeling resistance, N-vinyl cyclic amide, (meth)acrylamide, etc. are preferred. The nitrogen atom-containing monomer may be used alone or in combination of two or more kinds.
[0072] The N-vinyl cyclic amide is preferably one represented by the following formula (10):
[0073] In formula (10), R 101 is a divalent organic group, preferably a divalent saturated or unsaturated hydrocarbon group, and more preferably a divalent saturated hydrocarbon group (e.g., an alkylene group having 3 to 5 carbon atoms). 101 are directly bonded via a single bond to form a ring structure.
[0074] As the N-vinyl cyclic amide represented by formula (10), from the viewpoint of improving foaming and peeling resistance, N-vinyl-2-pyrrolidone (NVP), N-vinyl-2-piperidone, N-vinyl-2-caprolactam, N-vinyl-3-morpholinone, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, and the like are preferred, more preferably N-vinyl-2-pyrrolidone and N-vinyl-2-caprolactam, and even more preferably N-vinyl-2-pyrrolidone.
[0075] Examples of (meth)acrylamides include (meth)acrylamide, N-alkyl(meth)acrylamide, N,N-dialkyl(meth)acrylamide, etc. Examples of N-alkyl(meth)acrylamides include N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-n-butyl(meth)acrylamide, N-octylacrylamide, etc. N-alkyl(meth)acrylamides also include (meth)acrylamides having an amino group, such as dimethylaminoethyl(meth)acrylamide, diethylaminoethyl(meth)acrylamide, and dimethylaminopropyl(meth)acrylamide.
[0076] Examples of N,N-dialkyl(meth)acrylamides include N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, and N,N-di(t-butyl)(meth)acrylamide.
[0077] (Meth)acrylamides also include, for example, various N-hydroxyalkyl(meth)acrylamides, such as N-methylol(meth)acrylamide, N-(2-hydroxyethyl)(meth)acrylamide, N-(2-hydroxypropyl)(meth)acrylamide, N-(1-hydroxypropyl)(meth)acrylamide, N-(3-hydroxypropyl)(meth)acrylamide, N-(2-hydroxybutyl)(meth)acrylamide, N-(3-hydroxybutyl)(meth)acrylamide, N-(4-hydroxybutyl)(meth)acrylamide, and N-methyl-N-2-hydroxyethyl(meth)acrylamide.
[0078] (Meth)acrylamides also include, for example, various N-alkoxyalkyl(meth)acrylamides, such as N-methoxymethyl(meth)acrylamide and N-butoxymethyl(meth)acrylamide.
[0079] Examples of nitrogen atom-containing monomers other than N-vinyl cyclic amides and (meth)acrylamides include amino group-containing monomers such as aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate; cyano group-containing monomers such as acrylonitrile and methacrylonitrile; (meth)acryloylmorpholine, N-vinylpiperazine, N-vinylpyrrole, N-vinylimidazole, N-vinylpyrazine, N-vinylmorpholine, N-vinylpyrazole, vinylpyridine, vinylpyrimidine, vinyloxazole, vinylisoxazole, vinylthiazole, vinylisothiazole, vinylpyridazine, (meth)acryloylpyrrolidone, (meth)acryloylpyrrolidine, (meth)acryloylpiperidine, N-methyl Examples of the monomer include heterocycle-containing monomers such as vinylpyrrolidone; maleimide-based monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide; itaconimide-based monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-laurylitaconimide, and N-cyclohexylitaconimide; and imide group-containing monomers such as succinimide-based monomers such as N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, and N-(meth)acryloyl-8-oxyoctamethylenesuccinimide; and isocyanate group-containing monomers such as 2-(meth)acryloyloxyethylisocyanate.
[0080] The content of the nitrogen atom-containing monomer in the monomer group is, for example, 40% by weight or less, and may be 35% by weight or less, 30% by weight or less, 25% by weight or less, 20% by weight or less, 15% by weight or less, 13% by weight or less, 10% by weight or less, 8% by weight or less, 6% by weight or less, or even 5% by weight or less. The lower limit of the content is, for example, 0.5% by weight or more, and may be 1% by weight or more, 2% by weight or more, 3% by weight or more, 4% by weight or more, 5% by weight or more, 7% by weight or more, or even 10% by weight or more. The monomer group may not contain a nitrogen atom-containing monomer.
[0081] The monomer group may include monomers other than those mentioned above.
[0082] In the photocurable composition, each of the above-mentioned monomers may be contained as a partial polymer. The partial polymer may be either a homopolymer or a copolymer. The photocurable composition may not contain a partial polymer.
[0083] The photocurable composition may contain a crosslinking agent. An example of the crosslinking agent is a polyfunctional monomer having two or more polymerizable functional groups in one molecule. The polyfunctional monomer may be a (meth)acrylic monomer. Examples of the polyfunctional monomer are a monomer having two or more C=C bonds in one molecule, and a monomer having one or more C=C bonds and one or more polymerizable functional groups such as epoxy groups, aziridine groups, oxazoline groups, hydrazine groups, methylol groups, etc. in one molecule. The polyfunctional monomer is preferably a monomer having two or more C=C bonds in one molecule.
[0084] Examples of the polyfunctional monomer include (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,2-ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol diacrylate (N Polyfunctional acrylates (e.g., ester compounds of polyhydric alcohols and (meth)acrylic acid) such as 1,12-dodecanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and tetramethylolmethane tri(meth)acrylate; allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, butyl di(meth)acrylate, and hexyl di(meth)acrylate. The polyfunctional monomer is preferably a polyfunctional acrylate, and more preferably 1,9-nonanediol diacrylate, trimethylolpropane tri(meth)acrylate, hexanediol di(meth)acrylate, or dipentaerythritol hexa(meth)acrylate.
[0085] The amount of crosslinking agent to be added varies depending on the molecular weight, the number of functional groups, etc., but may be, for example, 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, 0.5 parts by weight or less, or even 0.3 parts by weight or less, relative to 100 parts by weight of the total of the monomer group and its partial polymer. The lower limit of the amount to be added may be, for example, 0.01 parts by weight or more, or even 0.05 parts by weight or more. The photocurable composition may not contain a crosslinking agent.
[0086] The photocurable composition may contain additives other than those described above. Examples of the additives include a chain transfer agent, a silane coupling agent, a viscosity modifier, a tackifier, a plasticizer, a softener, an antioxidant, a filler, a colorant, an antioxidant, a surfactant, an antistatic agent, and an ultraviolet absorber. The photocurable composition may not contain any additives.
[0087] The viscosity of the photocurable composition is preferably 5 to 100 poise. Photocurable compositions having a viscosity in the above range are particularly suitable for forming pressure-sensitive adhesive sheets.
[0088] The solvent content in the photocurable composition is, for example, 5 wt% or less, and may be 4 wt% or less, 3 wt% or less, 2 wt% or less, 1 wt% or less, or even 0.5 wt% or less. The photocurable composition may be substantially free of solvent. "Substantially free of solvent" means that solvents derived from additives and the like are allowed in a content of, for example, 0.1 wt% or less, preferably 0.05 wt% or less, and more preferably 0.01 wt% or less.
[0089] [Adhesive Sheet] An example of the adhesive sheet of this embodiment is shown in Fig. 1. The adhesive sheet 1 of Fig. 1 is a sheet formed from the photocurable composition of this embodiment.
[0090] The polymerization rate of the monomer group in the pressure-sensitive adhesive sheet 1 is, for example, 90% or more, and may be 91% or more, 92% or more, 93% or more, 94% or more, 95% or more, 96% or more, 97% or more, 98% or more, 98.5% or more, 99% or more, or even 99.5% or more. The upper limit of the polymerization rate is, for example, 99.99% or less.
[0091] The content (residual amount) of the photopolymerization initiator in the pressure-sensitive adhesive sheet 1 is, for example, 800 wtppm or less, 750 wtppm or less, 700 wtppm or less, 650 wtppm or less, 600 wtppm or less, 550 wtppm or less, 500 wtppm or less, 450 wtppm or less, 400 wtppm or less, 380 wtppm or less, 350 wtppm or less, 330 The residual amount may be 0 wtppm or less, 300 wtppm or less, 280 wtppm or less, 250 wtppm or less, 230 wtppm or less, 200 wtppm or less, 180 wtppm or less, 150 wtppm or less, 130 wtppm or less, 100 wtppm or less, 80 wtppm or less, 50 wtppm or less, 30 wtppm or less, or even 25 wtppm or less. The lower limit of the content is 0 wtppm or more. The reduced residual amount can contribute to suppressing yellowing and foaming in the pressure-sensitive adhesive sheet 1. It can also contribute to suppressing changes in the adhesive strength of the pressure-sensitive adhesive sheet 1 over time and suppressing heavy release of the release liner (particularly the release liner on the side irradiated with light such as ultraviolet light) during the formation of the pressure-sensitive adhesive sheet 1.
[0092] The pressure-sensitive adhesive sheet 1 can achieve an increased polymerization rate and a reduced residual amount of photopolymerization initiator. The polymerization rate of the monomer group in the pressure-sensitive adhesive sheet 1 may be 96% or more, and the content of the photopolymerization initiator may be 800 wtppm or less. The polymerization rate and content may each be within the above-mentioned numerical ranges. The content of the photopolymerization initiator in the pressure-sensitive adhesive sheet 1 can be evaluated by liquid chromatography.
[0093] The polymerization rate and content of the photopolymerization initiator in the pressure-sensitive adhesive sheet 1 may satisfy the formula: content of photopolymerization initiator (wtppm)≦233×polymerization rate (%)−22200.
[0094] The weight-average molecular weight (Mw) of the polymer contained in the pressure-sensitive adhesive sheet 1 is, for example, 500,000 or more, and may be 600,000 or more, 650,000 or more, 700,000 or more, 750,000 or more, 800,000 or more, 850,000 or more, or even 900,000 or more. The upper limit of Mw is not particularly limited and may be, for example, 3,000,000 or less. A pressure-sensitive adhesive sheet 1 containing a polymer having an Mw within the above range is suitable for suppressing peeling of the pressure-sensitive adhesive sheet 1 from an adhesive target, such as in a high-temperature environment. The adhesive target is, for example, an optical film. An example of an optical film is a polarizing film. The number-average molecular weight (Mn) of the polymer is, for example, 150,000 or more, and may be 170,000 or more, 180,000 or more, 190,000 or more, or even 200,000 or more. The upper limit of Mn is not particularly limited and may be, for example, 600,000 or less. Mw / Mn, which refers to the molecular weight distribution, is, for example, 1.8 to 10, 1.8 to 7, or even 1.8 to 5. Mw and Mn are determined from values measured by GPC (gel permeation chromatography) and calculated in terms of polystyrene.
[0095] The gel fraction of the pressure-sensitive adhesive sheet 1 is, for example, 50% or more, and may be 75% or more, 80% or more, or even 85% or more.
[0096] The thickness of the pressure-sensitive adhesive sheet 1 is, for example, 2 to 500 μm, and may be 2 to 300 μm, 2 to 200 μm, or even 2 to 150 μm. The upper limit of the thickness may be 100 μm or less, 70 μm or less, 60 μm or less, 50 μm or less, 40 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the thickness may be 5 μm or more, 10 μm or more, or even 15 μm or more.
[0097] The pressure-sensitive adhesive sheet 1 can be used in, for example, an optical laminate or an image display device, but the uses of the pressure-sensitive adhesive sheet 1 are not limited to the above examples.
[0098] (Method of manufacturing pressure-sensitive adhesive sheet) The pressure-sensitive adhesive sheet 1 can be formed, for example, by irradiating light 14 onto a first laminate 10 including, in this order, a base sheet 11, a coating layer 12 containing the photocurable composition of the present embodiment, and a release liner 13 (see FIG. 2 ). The coating layer 12 is irradiated with light 14 and cured to form the pressure-sensitive adhesive sheet 1. Irradiation with light 14 is typically carried out from the side of the base sheet 11. In this case, the light 14 passes through the base sheet 11 and reaches the coating layer 12, curing the coating layer 12. However, irradiation with light 14 may also be carried out from the side of the release liner 13, or from both the side of the release liner 13 and the side of the base sheet 11.
[0099] The formed pressure-sensitive adhesive sheet 1 is sandwiched between the base sheet 11 and the release liner 13 until the release liner 13 is peeled off, and constitutes part of the second laminate 17. By peeling the release liner 13 from the second laminate 17, a third laminate 15 including the base sheet 11 and the pressure-sensitive adhesive sheet 1 is obtained. In the third laminate 15, the surface of the pressure-sensitive adhesive sheet 1 is exposed to the outside. An optical film can be laminated onto the exposed surface of the pressure-sensitive adhesive sheet 1 directly or via another layer.
[0100] The light 14 is, for example, visible light or ultraviolet light having a wavelength shorter than 450 nm. The light may include light having a wavelength in the same range as the absorption wavelength of the photopolymerization initiator contained in the photocurable composition. Light having a wavelength of 300 nm or less and cut out using a filter or the like may be irradiated. Cutting out short-wavelength light is suitable for suppressing deterioration of the base sheet 11 and / or the release liner 13 due to the light 14. The light source 18 of the light 14 is, for example, a light irradiation device equipped with an ultraviolet irradiation lamp. Examples of ultraviolet irradiation lamps include ultraviolet LEDs, low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, xenon lamps, microwave-excited mercury lamps, black light lamps, chemical lamps, germicidal lamps, low-pressure discharge mercury lamps, and excimer lasers. Two or more ultraviolet irradiation lamps may be combined. Using ultraviolet LEDs allows the wavelength band of the irradiated ultraviolet light to be narrower than when using other light sources.
[0101] The light source 18 may be an LED. Compared to black light sources, LEDs not only allow for easier adjustment of illuminance, but also tend to have a longer light source life. Compared to black light sources that use mercury, LEDs are also superior in terms of reducing environmental impact. When using an ultraviolet LED as the light source, an LED with a peak wavelength of 325 to 350 nm may be selected. According to the inventors' studies, the use of an LED with a peak wavelength of 325 to 350 nm may contribute to improving the polymerization rate of the monomer group in the pressure-sensitive adhesive sheet 1 and / or reducing the amount of residual photopolymerization initiator compared to, for example, the use of a black light source. Furthermore, LEDs that emit light 14 with a peak wavelength of 325 to 350 nm tend to generate less heat and make it easier to control the temperature of the coating layer 12 compared to LEDs that emit light with a peak wavelength of approximately 365 nm. To the best of the inventors' knowledge, no examples have been reported of producing pressure-sensitive adhesive sheets using LEDs that emit light with a peak wavelength of 325 to 350 nm.
[0102] As the LED having a peak wavelength in the range of 325 to 350 nm, an LED having a peak wavelength of 340±10 nm (hereinafter referred to as LED 340) may be selected.
[0103] Focusing on the peak wavelength of the light 14, the peak wavelength of the light 14 irradiated onto the first laminate 10 (specifically, the coating layer 12) may be 325 nm to 350 nm. The peak wavelength of the light 14 is preferably 340±10 nm (330 nm to 350 nm), may be 340±5 nm (335 nm to 345 nm), may be 340±2 nm (338 nm to 342 nm), or may be 340 nm. The peak wavelength refers to the wavelength at which the intensity of the light 14 reaches a maximum value in a spectrum showing the relationship between the wavelength and intensity of the light 14. The light 14 may further have a peak wavelength in a wavelength range other than 325 nm to 350 nm, but preferably does not have such a peak wavelength.
[0104] The illuminance of the light 14 irradiated onto the first laminate 10 (specifically, the coating layer 12) is, for example, 2.0 to 30 mW / cm 2 The illuminance is 2.5 mW / cm 2 Above, 3.0mW / cm2 Above, 3.5mW / cm 2 Above, 4.0mW / cm 2 Above, 5.0mW / cm 2 Above, 6.0mW / cm 2 Above, 7.0mW / cm 2 Above, 8.0mW / cm 2 Above, 9.0mW / cm 2 or more, and even 10 mW / cm 2 The upper limit of the illuminance may be, for example, 25 mW / cm 2 less than 20 mW / cm 2 Below 15mW / cm 2 It may be the following:
[0105] The time for irradiating the first laminate 10 (specifically, the coating layer 12) with the light 14 is, for example, 10 to 1,000 seconds, and may be 60 seconds or more, 100 seconds or more, 150 seconds or more, or even 200 seconds or more. The upper limit of the time is, for example, 800 seconds or less, and may be 600 seconds or less, 500 seconds or less, 400 seconds or less, 300 seconds or less, or even 250 seconds or less. The irradiation with the light 14 may be continuous or intermittent.
[0106] The integrated light amount of the light 14 on the first laminate 10 (specifically, the coating layer 12) is, for example, 25 mJ / cm 2 or more, and 100 mJ / cm 2 Above, 500mJ / cm 2 Above, 1000mJ / cm 2 Above, 2000mJ / cm 2 Above, 2500mJ / cm 2 or more, and even 3000 mJ / cm 2 The upper limit of the integrated light amount is not particularly limited, and may be, for example, 30,000 mJ / cm 2 or less, and 10,000 mJ / cm 2 Below, 5000mJ / cm 2 Below 4000 mJ / cm 2 It may be the following:
[0107] An example of the substrate of the release liner 13 (hereinafter referred to as "liner substrate") is a resin film. Examples of resins that can be contained in the liner substrate include polyesters such as polyethylene terephthalate and polyethylene naphthalate, acetate resins, polyethersulfone, polycarbonate, polyamide, polyimide, polyolefin, (meth)acrylic resins, polyvinyl chloride, polyvinylidene chloride, polystyrene, polyvinyl alcohol, polyarylate, and polyphenylene sulfide. The resin is preferably a polyester such as polyethylene terephthalate.
[0108] The release liner 13 may include a layer other than the liner substrate. The release liner 13 may include a release layer. The release liner 13 includes, for example, a liner substrate and a release layer formed on one surface of the liner substrate. This release liner 13 can be used so that the release layer faces the coating layer 12. The release layer is typically a cured layer of a release agent composition containing a release agent. Various release agents can be used as the release agent, such as silicone-based release agents, fluorine-based release agents, long-chain alkyl-based release agents, fatty acid amide-based release agents, and silica powder.
[0109] The release liner 13 may be in the form of a sheet or a continuous piece.
[0110] An example of the substrate sheet 11 is a resin film. Examples of the resin contained in the substrate sheet 11 are the same as the examples of the resin that can be contained in the liner substrate.
[0111] The thickness of the base sheet 11 is, for example, 10 to 200 μm, and may be 25 to 150 μm.
[0112] The base sheet 11 may have a release layer on the surface facing the coating layer 12. Examples of the release layer that may be provided on the base sheet 11 are the same as the examples of the release layer that may be provided on the release liner 13. Both the release liner 13 and the base sheet 11 may have a release layer.
[0113] For the base sheet 11 , a sheet having a greater peel strength from the pressure-sensitive adhesive sheet 1 than the release liner 13 can usually be selected.
[0114] The base sheet 11 may be in the form of a sheet or a continuous sheet.
[0115] The first laminate 10 can be formed, for example, by forming a coating layer 12 on a base sheet 11 (or a release liner 13) and then placing the release liner 13 (or base sheet 11) on the formed coating layer 12. Alternatively, the first laminate 10 may be formed by applying the photocurable composition in a poured manner into the space between the base sheet 11 and the release liner 13, which are held at a predetermined distance so that their main surfaces face each other.
[0116] The coating layer 12 can be formed by various coating methods such as roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating.
[0117] The thickness of the coating layer 12 can be adjusted depending on the desired thickness of the PSA sheet 1, and may be, for example, 2 to 500 μm, 2 to 300 μm, 2 to 200 μm, or even 2 to 150 μm. The upper limit of the thickness may be 100 μm or less, 70 μm or less, 60 μm or less, 50 μm or less, 40 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the thickness may be 5 μm or more, 10 μm or more, or even 15 μm or more.
[0118] The first laminate 10 may include a long base sheet 11, a long coating layer 12, and a long release liner 13, or in other words, may be long. The long first laminate 10 can be obtained, for example, by forming the coating layer 12 between the base sheet 11 and the release liner 13 while conveying them after they have been unwound from a roll.
[0119] As described above, the present invention further provides a method for producing a pressure-sensitive adhesive sheet, comprising irradiating a coating layer of a photocurable composition containing a monomer group and / or a partial polymer of the monomer group, and a photopolymerization initiator having chemical structure X in its molecule with light 14 to photocure the coating layer.
[0120] [Optical laminate] An example of the optical laminate of this embodiment is shown in Fig. 3. The optical laminate 20A in Fig. 3 includes a pressure-sensitive adhesive sheet 1 and an optical film 2. The pressure-sensitive adhesive sheet 1 and the optical film 2 are laminated to each other. The optical laminate 20A can be used as an optical film with a pressure-sensitive adhesive sheet.
[0121] Examples of the optical film 2 include a polarizing film, a retardation film, and a laminate film including a polarizing film and / or a retardation film. However, the optical film 2 is not limited to the above examples. The optical film 2 may also include a glass film.
[0122] The optical film 2 may be a polarizing film, and the pressure-sensitive adhesive sheet 1 may be in contact with the optical film 2 .
[0123] The polarizing film includes a polarizer. The polarizing film typically includes a polarizer and a protective film (transparent protective film). The protective film is disposed, for example, in contact with a main surface (the surface having the largest area) of the polarizer. The polarizer may be disposed between two protective films. The protective film may be disposed on at least one surface of the polarizer.
[0124] The polarizer is not particularly limited, and examples thereof include a hydrophilic polymer film such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, or an ethylene-vinyl acetate copolymer partially saponified film, which has been uniaxially stretched after adsorbing a dichroic substance such as iodine or a dichroic dye; a polyene-based oriented film such as a dehydrated polyvinyl alcohol or a dehydrochlorinated polyvinyl chloride; etc. A polarizer typically comprises a polyvinyl alcohol film (polyvinyl alcohol films include an ethylene-vinyl acetate copolymer partially saponified film) and a dichroic substance such as iodine.
[0125] The thickness of the polarizer is not particularly limited and may be, for example, 80 μm or less, 50 μm or less, 30 μm or less, 25 μm or less, or even 20 μm or less. The lower limit of the polarizer thickness is not particularly limited and may be, for example, 1 μm or more, 5 μm or more, 10 μm or more, or even 15 μm or more. A thin polarizer (for example, a thickness of 20 μm or less) is suppressed in dimensional change and can contribute to improving the durability of the optical laminate, particularly durability at high temperatures.
[0126] The material for the protective film may be, for example, a thermoplastic resin having excellent transparency, mechanical strength, thermal stability, moisture-blocking properties, isotropy, etc. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The material for the protective film may be a thermosetting resin or an ultraviolet-curable resin such as a (meth)acrylic, urethane, acrylic urethane, epoxy, or silicone-based resin. When the polarizing film has two protective films, the materials of the two protective films may be the same or different. For example, a protective film made of a thermoplastic resin may be bonded to one main surface of the polarizer via an adhesive, and a protective film made of a thermosetting resin or an ultraviolet-curable resin may be bonded to the other main surface of the polarizer. The protective film may contain one or more optional additives, such as ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, color inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants.
[0127] The thickness of the protective film can be determined as appropriate, but is generally about 10 to 200 μm in view of strength, workability such as handling, thinness, and the like.
[0128] The polarizer and the protective film are usually adhered to each other via an aqueous adhesive or the like. Examples of aqueous adhesives include isocyanate-based adhesives, polyvinyl alcohol-based adhesives, gelatin-based adhesives, vinyl latex, aqueous polyurethane, and aqueous polyester. Examples of adhesives other than the above-mentioned adhesives include ultraviolet-curable adhesives and electron beam-curable adhesives. Electron beam-curable polarizing film adhesives exhibit suitable adhesiveness to various protective films. The adhesive may contain a metal compound filler.
[0129] In the polarizing film, a retardation film or the like can be formed on the polarizer instead of the protective film. Another protective film or a retardation film or the like can be further provided on the protective film.
[0130] The protective film may have a hard coat layer on the surface opposite to the surface bonded to the polarizer, and may also be subjected to treatments for purposes such as anti-reflection, anti-sticking, diffusion, and anti-glare.
[0131] The polarizing film may be a circular polarizing film.
[0132] The thickness of the polarizing film is, for example, 500 μm or less, and may be 300 μm or less, 200 μm or less, 100 μm or less, or even 60 μm or less. The lower limit of the thickness may be, for example, 10 μm or more, 25 μm or more, or even 40 μm or more.
[0133] The retardation film is a film having birefringence in the in-plane direction and / or the thickness direction, and is, for example, a stretched resin film or a film in which a liquid crystal material is oriented and fixed.
[0134] The retardation film may be a λ / 4 plate, a λ / 2 plate, an anti-reflection retardation film (see, for example, paragraphs 0221, 0222, and 0228 of JP 2012-133303 A), a viewing angle compensation retardation film (see, for example, paragraphs 0225 and 0226 of JP 2012-133303 A), or an inclined orientation retardation film for viewing angle compensation (see, for example, paragraph 0227 of JP 2012-133303 A). The retardation film is not limited to the above examples as long as it has birefringence in the in-plane direction and / or the thickness direction. There are also no limitations on the retardation value, arrangement angle, three-dimensional birefringence, whether the retardation film is single-layer or multi-layer, etc. of the retardation film. Known films can be used as the retardation film.
[0135] The thickness of the optical film 2 is, for example, 1 to 200 μm.
[0136] The optical film 2 may be a single layer or a laminated film composed of two or more layers. When the optical film 2 is a laminated film, the pressure-sensitive adhesive sheet 1 may be used to bond the layers together.
[0137] Another example of the optical laminate of the present embodiment is shown in Fig. 4. The optical laminate 20B in Fig. 4 has a layered structure in which a release liner 3, a pressure-sensitive adhesive sheet 1, and an optical film 2 are layered in this order. By peeling off the release liner 3, the optical laminate 20B can be used as an optical film with a pressure-sensitive adhesive sheet.
[0138] The release liner 3 is typically a resin film. Examples of resins that make up the release liner 3 include polyesters such as polyethylene terephthalate (PET), polyolefins such as polyethylene and polypropylene, polycarbonate, acrylic, polystyrene, polyamide, and polyimide. The surface of the release liner 3 that comes into contact with the pressure-sensitive adhesive sheet 1 may be subjected to a release treatment. The release treatment is, for example, a treatment with a silicone compound. However, the release liner 3 is not limited to the above examples. The release liner 3 is peeled off when the optical laminate 20B is used, for example, when it is attached to the image forming layer.
[0139] Another example of the optical laminate of the present embodiment is shown in Fig. 5. The optical laminate 20C in Fig. 5 has a layered structure in which a release liner 3, a pressure-sensitive adhesive sheet 4, a retardation film 2B, a pressure-sensitive adhesive sheet 1, and a polarizing film 2A are layered in this order. After the release liner 3 is peeled off, the optical laminate 20C can be used by being attached to, for example, an image-forming layer.
[0140] A known adhesive sheet can be used as the adhesive sheet 4. The adhesive sheet 1 may also be used as the adhesive sheet 4.
[0141] Another example of the optical laminate of this embodiment is shown in Fig. 6. Optical laminate 20D in Fig. 6 has a layered structure in which a release liner 3, a pressure-sensitive adhesive sheet 4, a retardation film 2B, a pressure-sensitive adhesive sheet 1, a polarizing film 2A, and a protective film 5 are layered in this order. After peeling off the release liner 3, optical laminate 20D can be used by being attached to, for example, an image-forming layer.
[0142] The protective film 5 has the function of protecting the optical film 2 (polarizing film 2A), which is the outermost layer, during distribution and storage of the optical laminate 20D and when the optical laminate 20D is incorporated into an image display device. The protective film 5 may also function as a window to the external space when incorporated into an image display device. The protective film 5 is typically a resin film. Examples of resins constituting the protective film 5 include polyesters such as PET, polyolefins such as polyethylene and polypropylene, acrylics, cycloolefins, polyimides, and polyamides, with polyesters being preferred. However, the protective film 5 is not limited to the above examples. The protective film 5 may be a glass film or a laminate film including a glass film. The protective film 5 may be subjected to surface treatments such as anti-glare, anti-reflection, and anti-static.
[0143] The protective film 5 may be bonded to the optical film 2 by any adhesive. Bonding by an adhesive sheet 1 is also possible.
[0144] The optical laminate may have any configuration as long as it includes the pressure-sensitive adhesive sheet 1 and the optical film 2 .
[0145] The optical laminate of this embodiment can be distributed and stored, for example, as a rolled body obtained by rolling up a strip-shaped optical laminate, or as a sheet-shaped optical laminate.
[0146] The optical laminate of this embodiment is typically used in an image display device, such as a liquid crystal display, an organic EL display, or an inorganic EL display.
[0147] [Image Display Device] An example of an image display device according to this embodiment is shown in Figure 7. The image display device 21 in Figure 7 has a layered structure in which a substrate 7, an image forming layer (e.g., an organic EL layer or a liquid crystal layer) 6, a pressure-sensitive adhesive sheet 4, a retardation film 2B, a pressure-sensitive adhesive sheet 1, a polarizing film 2A, and a protective film 5 are layered in this order. The image display device 21 has the optical laminates 20A, 20B, 20C, and 20D shown in Figures 3 to 6 (excluding the release liner 3). The substrate 7 and the image forming layer 6 may have the same configurations as the substrate and the image forming layer, respectively, of known image display devices.
[0148] The image display device 21 in Fig. 7 may be an organic EL display or a liquid crystal display. However, the image display device 21 is not limited to this example. The image display device 21 may be an electroluminescence (EL) display, a plasma display (PD), a field emission display (FED), or the like. The image display device 21 may be used for home appliances, in-vehicle applications, public information displays (PID), and the like.
[0149] The image display device 21 may have any configuration as long as it includes the pressure-sensitive adhesive sheet 1 and / or the optical laminate 20 .
[0150] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the examples shown below.
[0151] [Monomer Syrup A1] 95.2 parts by weight of n-butyl acrylate (BA), 4.75 parts by weight of acrylic acid (AA), 0.05 parts by weight of 4-hydroxybutyl acrylate (HBA), and 0.2 parts by weight of 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)2-methylpropan-1-one (Omnirad 127, manufactured by IGM Resins) as a photopolymerization initiator were placed in a four-neck flask. Next, the liquid in the flask was irradiated with ultraviolet light under a nitrogen atmosphere to obtain Monomer Syrup A1, in which the monomers were partially photopolymerized. UV irradiation was continued until the viscosity of the liquid in the flask (measurement conditions: BH viscometer No. 5 rotor, 10 rpm, measurement temperature 30°C) reached approximately 20 Pa s.
[0152] [Monomer Syrups A2 to A14] Monomer syrups A2 to A14 were prepared in the same manner as for Monomer Syrup A1, except that the monomers and photopolymerization initiators were changed as shown in Table 1.
[0153]
[0154] The abbreviations in Table 1 are as follows: BA: n-butyl acrylate AA: acrylic acid HBA: 4-hydroxybutyl acrylate Omnirad 127: 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)2-methylpropan-1-one (Omnirad 127, manufactured by IGM Resin) Omnirad 1173: 2-hydroxy-2-methyl-1-phenylpropanone (Omnirad 1173, manufactured by IGM Resin) Omnirad 184: 1-hydroxycyclohexyl-phenyl ketone (Omnirad 184, manufactured by IGM Resin) Omnirad 651: 2,2-dimethoxy-1,2-diphenylethan-1-one (Omnirad 651, manufactured by IGM Resin) Omnirad 819: bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad 819, manufactured by IGM Resins) Omnirad 907: 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one (Omnirad 907, manufactured by IGM Resins)
[0155] Omnirad 184, Omnirad 651, Omnirad 819 and Omnirad 907 do not have the chemical structure X in their molecules.
[0156] [Photocurable Compositions C1 to C14] Next, the monomer syrup, the monomer, and the crosslinking agent were mixed so as to have the compositions shown in Table 2 below, thereby obtaining photocurable compositions C1 to C14.
[0157]
[0158] The abbreviations in Table 2 are as follows: AA: acrylic acid NVP: N-vinyl-2-pyrrolidone NDDA: 1,9-nonanediol diacrylate
[0159] The final compositions of the monomers contained in photocurable compositions C13 and C14 are shown in Table 3 below.
[0160]
[0161] The abbreviations in Table 3 are as follows: BA: n-butyl acrylate AA: acrylic acid HBA: 4-hydroxybutyl acrylate NVP: N-vinyl-2-pyrrolidone
[0162] Example 1 Preparation of Release Liner A silicone-based release agent composition was obtained by mixing 30 parts by weight of an addition reaction curable silicone (LTC761 containing a hexenyl group-containing polyorganosiloxane, a 30 wt % toluene solution, manufactured by Dow Corning Toray), 0.9 parts by weight of a release control agent (BY24-850 containing an unreactive silicone resin, manufactured by Dow Corning Toray), and 2 parts by weight of a curing catalyst (SRX212 containing a platinum catalyst, manufactured by Dow Corning Toray), and a toluene / hexane mixed solvent (volume ratio 1:1) as a dilution solvent. The silicone solids concentration in the release agent composition was 1.0 wt %. Next, the release agent composition was applied with a wire bar to one side of a liner substrate (Lumirror XD500P, a polyester film, 75 μm thick), and heated at 130° C. for 1 minute to prepare a release liner having a release layer (60 nm thick) on one side.
[0163] [Preparation of Pressure-Sensitive Adhesive Sheet] The photocurable composition C1 was applied to one side of a substrate sheet (Lumirror XD500P, a polyester film without a release layer, with a thickness of 75 μm) using an applicator to form a coating layer (thickness of 20 μm). Next, a release liner was placed on the formed coating layer to obtain a first laminate. The release liner was placed so that the release layer was in contact with the coating layer. Next, an illuminance of 4 mW / cm was applied from the substrate sheet side of the first laminate. 2 The coating layer was then photocured with light from an LED under the conditions of 1000 nm, 1000 s, and 200 s irradiation time. The peak wavelength of this light was 340 nm. This resulted in a photocuring of the coating layer, and a PSA sheet (thickness: 20 μm) of Example 1 sandwiched between the base sheet and the release liner was obtained. The illuminance of the light was measured using an illuminance meter (UD-T3040T2, manufactured by Topcon Technohouse Co., Ltd.) near the ultraviolet light incident surface of the base sheet.
[0164] (Examples 2 to 3, 9 to 10 and Comparative Example 1) Pressure-sensitive adhesive sheets of Examples 2 to 3, 9 to 10 and Comparative Example 1 were obtained by the same method as in Example 1, except that the photocurable composition used was changed as shown in Table 4.
[0165] (Examples 4 to 8 and Comparative Examples 2 to 5) The photocurable compositions used were changed as shown in Table 4, and the illuminance of the irradiated light was changed to 14 mW / cm 2 Except for the change in the temperature, pressure-sensitive adhesive sheets of Examples 4 to 8 and Comparative Examples 2 to 5 were obtained by the same method as in Example 1. In Example 7, an LED (LED365) having a peak wavelength at 365 nm was used as the light source.
[0166] [Polymerization Rate of Monomer Group] The polymerization rate of the monomer group in each PSA sheet of the Examples and Comparative Examples was calculated from the change in weight of the PSA sheet before and after 2 hours of heat drying at 130° C. Specifically, the weight of the PSA sheet immediately after peeling off the base sheet and release liner was defined as W0 (weight before drying), and the weight of the PSA sheet after cooling at room temperature (23° C.) for about 20 minutes after the heating was defined as W1 (weight after drying), and the polymerization rate was calculated using the formula: polymerization rate (%) = W1 / W0 × 100.
[0167] [Remaining amount of photopolymerization initiator] The composition of each pressure-sensitive adhesive sheet of the Examples and Comparative Examples was analyzed, and the remaining amount (content) of the photopolymerization initiator was calculated based on the results obtained. The composition analysis was performed using liquid chromatography (LC) under the following conditions. Instrument used: 1290 Infinity II (Agilent Technologies) Column: Acquity UPLC BEH C18 (Waters, 2.1 mmφ×100 mm, 1.7 μm) Eluent composition: ultrapure water / acetonitrile gradient conditions Column temperature: 40°C Column flow rate: 0.2 mL / min Injection volume: 2 μL Detector: photodiode array detector (PDA) Measurement wavelength: 190 to 400 nm Extraction wavelength: Omnirad 127 = 262 nm, Omnirad 1173 = 246 nm, Omnirad 184 = 246 nm, Omnirad 651 = 253 nm, Omnirad 819 = 296 nm, Omnirad 907 = 309 nm Sample preparation method: Approximately 0.5 g of sample (adhesive sheet) was weighed, 2 mL of chloroform was added, and the mixture was shaken overnight. 8 mL of methanol was added to the resulting solution, and the supernatant was filtered through a 0.45 μm membrane filter. The resulting filtrate was injected into an LC and analyzed.
[0168] The evaluation results are shown in Table 4 below, together with the type and amount of the photopolymerization initiator used.
[0169]
[0170] As shown in Table 4, when compared at similar polymerization rates, the pressure-sensitive adhesive sheets of the Examples formed from photocurable compositions containing a photopolymerization initiator having chemical structure X in the molecule exhibited reduced amounts of residual photopolymerization initiator compared to Comparative Examples 1 and 5. Furthermore, the pressure-sensitive adhesive sheets of Comparative Examples 2 to 4 exhibited polymerization rates less than 90%, resulting in excessive amounts of residual monomer. Figure 8 shows the relationship between polymerization rate and residual amount of photopolymerization initiator for each pressure-sensitive adhesive sheet of the Examples and Comparative Examples. As shown in Table 4 and Figure 8, the pressure-sensitive adhesive sheets of the Examples achieved higher polymerization rates and lower residual amounts of photopolymerization initiator compared to the pressure-sensitive adhesive sheets of the Comparative Examples. The dashed line in the graph of Figure 8 corresponds to the formula: photopolymerization initiator content (wtppm) = 233 × polymerization rate (%) - 22200. Comparative Examples 2 to 4 are located to the left of the dashed line in the graph.
[0171] <<Additional Examples>> [Monomer Syrups A15 to A17] Monomer syrups A15 to A17 were prepared in the same manner as Monomer Syrup A1, except that the monomers and photopolymerization initiators were changed as shown in Table 5. Table 5 also shows Monomer Syrup A1, which has the same monomer composition and photopolymerization initiator blending amount.
[0172]
[0173] [Photocurable Compositions C15 to C17] Next, photocurable compositions C15 to C17 were obtained by mixing monomer syrup and crosslinking agent to obtain the compositions shown in Table 6. Table 6 also shows photocurable composition C1, which has the same monomer composition of the monomer syrup and the same blending amount of photopolymerization initiator.
[0174]
[0175] (Examples 11 to 14) The photocurable compositions used were changed as shown in Table 7, and the illuminance of the irradiated light was changed to 9 mW / cm 2 Pressure-sensitive adhesive sheets of Examples 11 to 14 were obtained by the same method as in Example 1, except that the temperature was changed to 100°C. The polymerization rate of the monomer group and the amount of remaining photopolymerization initiator were evaluated for each of the obtained pressure-sensitive adhesive sheets by the same methods as in Examples 1 to 10. The evaluation results are shown in Table 7 below, together with the type and amount of photopolymerization initiator blended.
[0176]
[0177] As shown in Table 7, when compared at similar polymerization rates, the pressure-sensitive adhesive sheets of Examples 11 to 14 formed from photocurable compositions containing a photopolymerization initiator having chemical structure X in the molecule were able to reduce the amount of residual photopolymerization initiator compared to Comparative Examples 1 and 5. Furthermore, the relationship between the polymerization rate and the residual amount of photopolymerization initiator in the pressure-sensitive adhesive sheets of Examples 11 to 14 is located to the right of the dashed line shown in the graph of Figure 8.
[0178] The curable composition of the present invention can be used to form a pressure-sensitive adhesive sheet.
Claims
1. A photocurable composition for a pressure-sensitive adhesive sheet, comprising a monomer group and / or a partial polymer of the monomer group, and a photopolymerization initiator, wherein the photopolymerization initiator is a compound having a chemical structure shown in the following formula (1) in the molecule, R in the formula (1) 1 and R 2 are each independently a C1 to C8 alkyl group; -OH, a C1 to C4 alkoxy group, -CN, -COOR 51 , -OOCR 52 , or -NR 53 R 54 a C1-C4 alkyl group in which a hydrogen atom is replaced by; a C3-C6 alkenyl group; or -CH2-C6H4-R 55 And R 1 and R 2 may be bonded to each other to form a C2 to C9 alkylene group, a C3 to C6 oxyalkylene group, or an azaalkylene group, and X is -OR 56 , or -NR 57 R 58 And R 51 is a C1 to C8 alkyl group; R 52 is a C1-C4 alkyl group; R 53 and R 54 are each independently a hydrogen atom, a C1 to C12 alkyl group; -OH, a C1 to C4 alkoxy group, -CN and -COOR 59 a C2-C4 alkyl group, the hydrogen atom of which is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group; 53 and R 54 are bonded to each other to form -O- or -N(R 60 )-, and R may be a C3-C9 alkylene group optionally interrupted by -. 55 is a C1-C4 alkyl group; R 56 is a hydrogen atom, -SiR 62 3. A C1-C8 alkyl group or a C3-C6 alkenyl group; R 57 and R 58represents an alkyl group having 1 to 12 carbon atoms; —OH, an alkoxy group having 1 to 4 carbon atoms, —CN, and —COOR 63 a C2-C4 alkyl group, the hydrogen atom of which is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; or a cyclohexyl group; 57 and R 58 are bonded to each other to form -O- or -N(R 64 )-, and R may be a C3-C9 alkylene group optionally interrupted by -. 59 is a C1-C4 alkyl group; R 60 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an allyl group, a hydroxyalkyl group having 1 to 4 carbon atoms, -CH2CH2-COOR 61 or -CH2CH2CN, R 61 is a C1-C4 alkyl group; R 62 is a C1 to C6 alkyl group; R 63 is a C1-C4 alkyl group; R 64 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an allyl group, a hydroxyalkyl group having 1 to 4 carbon atoms, -CH2CH2-COOR 65 or -CH2CH2CN, R 65 is a C1 to C4 alkyl group, and the chemical structure can be bonded to a hydrogen atom or a hydrogen atom-substituted structure via the carbon atom marked with * in formula (1).
2. The above R 1 and the R 2 The photocurable composition of claim 1, wherein each of the groups is independently a C1 to C8 alkyl group.
3. The above R 1 and the R 2 The photocurable composition of claim 1 , wherein:
4. The X is -OR 56 2. The photocurable composition of claim 1, wherein 5. The photocurable composition of claim 1, wherein said X is --OH.
6. The photocurable composition according to claim 1, wherein the chemical structure is the structure shown in formula (2) below.
7. The photocurable composition according to claim 1, wherein the photopolymerization initiator is a compound having two or more of the above chemical structures in one molecule.
8. The photopolymerization initiator is a compound represented by the following formula (3), wherein R in the formula (3) 1 ' and R 2 ' are each other and the R 1 and R 2 Independently of R 1 and R 2 X′ is, independently of X, a group which may be taken as X; A is —O—, —CYR 3 - or -C(CH3)R 4 Y is a hydrogen atom, -Cl, -Br, -O-R 71 , -NR 72 R 73 , or -S-R 74 And R 3 is a hydrogen atom, a C1-C8 alkyl group, a C3-C6 alkenyl group, a benzyl group, -CH2-C6H4-R 75 or a phenyl group, R 4 is a C1-C6 alkyl or alkylene group, the alkylene group being bonded to a carbon atom of the phenylene group of the compound of formula (3); R 71 is a hydrogen atom, -Si(R 76 ) 3, C1-C12 alkyl group, C2-C18 acyl group, —CO—NH—R 77 , a C2 to C20 hydroxyalkyl group, a C2 to C20 methoxyalkyl group, 3-R 78 -2-hydroxypropyl group, 3-[1,3,3,3-tetramethyl-1-[(trimethylsilyl)oxy]disiloxanyl]propyl group, 2,3-dihydroxypropyl group, or a C2-C21 hydroxyalkyl group or a C3-C25 alkyl group, the carbon chain of which is interrupted by 1 to 9 oxygen atoms, R 72 and R 73 are each independently a C1 to C12 alkyl group; -OH, a C1 to C4 alkoxy group, -CN, and -COOR 79a C2-C4 alkyl group, the hydrogen atom of which is substituted with at least one group selected from the group consisting of: a C3-C5 alkenyl group; a cyclohexyl group; or a C7-C9 phenylalkyl group; 72 and R 73 are bonded to each other to form -O- or -N(R 80 )-, and R may be a C3-C9 alkylene group optionally interrupted by -. 74 represents an alkyl group having 1 to 18 carbon atoms, a hydroxyethyl group, a 2,3-dihydroxypropyl group, a cyclohexyl group, a benzyl group, a phenyl group, an alkylphenyl group having 1 to 12 carbon atoms, -CH2-COOR 81 -CH2CH2-COOR 82 or -CH(CH3)-COOR 83 And R 75 is a C1-C4 alkyl group; R 76 is a C1 to C6 alkyl group; R 77 is a C1 to C12 alkyl group; R 78 is a C1 to C18 alkoxy group; R 79 is a C1-C4 alkyl group; R 80 is a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, an allyl group, a benzyl group, a hydroxyalkyl group having 1 to 4 carbon atoms, -CH2CH2-COOR 84 or -CH2CH2CN, R 81 , R 82 and R 83 are each independently a C1 to C18 alkyl group; R 84 The photocurable composition according to claim 1, wherein is a C1 to C4 alkyl group.
9. The A is -CYR 3 The photocurable composition according to claim 8, wherein 10. The above Y and R 3 The photocurable composition according to claim 9 , wherein is a hydrogen atom.
11. The photocurable composition according to claim 8, wherein the photopolymerization initiator is a compound represented by the following formula (4):
12. The photocurable composition according to claim 1, wherein the amount of the photopolymerization initiator in the photocurable composition is 0.01 to 1 part by weight per 100 parts by weight of the total of the monomer group and the partially polymerized product.
13. The photocurable composition according to claim 1, wherein the monomer group includes a (meth)acrylic monomer.
14. An adhesive sheet formed from the photocurable composition according to claim 1.
15. The adhesive sheet according to claim 14, wherein the polymerization rate of the monomer group in the adhesive sheet is 96% or more, and the content of the photopolymerization initiator is 800 wtppm or less.
16. The pressure-sensitive adhesive sheet according to claim 14, wherein the thickness of the pressure-sensitive adhesive sheet is 300 μm or less.
17. An optical laminate comprising the pressure-sensitive adhesive sheet according to any one of claims 14 to 16 and an optical film.
18. The optical laminate according to claim 17, wherein the optical film is a polarizing film, and the pressure-sensitive adhesive sheet is in contact with the polarizing film.
19. An image display device comprising the optical laminate according to claim 17.
Citation Information
Patent Citations
Ultraviolet curable adhesive composition
JP2017101153A
Active energy ray-curable adhesive composition
JP2018199773A
Masking tape for forming electromagnetic wave shield
JP2019123833A
Web take-up roll with web edge treatment with printable adhesive composition
JP2019508534A
Active energy ray-curable adhesive composition for packaging material
JP2020083980A
Cited By
Photohardenable compositions and methods for use in volumetric three-dimensional printing
WO2025160576A1