Pellet, method for producing molded article, and film

By using polyolefin pellets with a laser marking agent and controlled angle of repose, the method addresses the issue of uneven printing in laser-printable products, achieving consistent and high-quality markings across containers and films.

WO2024203395A1PCT designated stage expired Publication Date: 2024-10-03TOYOBO CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010031
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-14
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing methods for manufacturing laser-printable containers and films often result in uneven printing due to variations in the concentration of laser marking agents, leading to inconsistent marking quality across products.

Method used

Developing polyolefin pellets with a laser marking agent and an angle of repose between 25 and 45 degrees, which are mixed with other pellets to ensure consistent supply and concentration, reducing variations in the extrusion process and resulting in more uniform laser printing across molded products such as containers and films.

Benefits of technology

The solution effectively suppresses variations in the concentration of the laser marking agent, reducing printing unevenness in both container-to-container and film-to-film applications, ensuring consistent and high-quality laser printing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

A purpose is to provide pellets capable of producing molded articles (for example, containers and films) able to reduce the uneven printing that can occur when laser printing is performed. Another purpose is to provide a method for producing a molded article capable of reducing the uneven printing that can occur when laser printing is performed. Another purpose is to provide a film capable of reducing the uneven printing that can occur when laser printing is performed. The pellets contain a polyolefin and a laser marking agent and have an angle of repose of 25-45° inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

Pellets, manufacturing method of molded product, and film

[0001] The present invention relates to pellets, a method for producing a molded article, and a film.

[0002] Laser-markable containers are known as food and beverage containers (see Patent Documents 1 to 3). Patent Document 1 describes a laser-markable pouch. Patent Document 2 describes a laser-markable laminated tube container. Patent Document 3 describes a laser-markable multilayer resin container. The manufacturing date, expiration date, lot number, etc. of the food and beverage can be marked on these containers using a laser.

[0003] Laser-printable films, labels, and lids are also known (see Patent Document 4). By printing information on these with a laser, it is possible to add the date of manufacture, expiration date, lot number, and the like.

[0004] To produce these, it is known to prepare pellets containing a laser marking agent, i.e., a masterbatch, and then mix the masterbatch with pellets that do not contain the laser marking agent (e.g., commercially available polyolefin pellets), and feed the mixture into an extruder (see, for example, Patent Document 4).

[0005] Patent No. 4727414 Patent No. 6592926 Patent No. 6260265 WO / 2021 / 125135A1

[0006] The inventors discovered that when a roll of film having a certain length (specifically, 500 m) is manufactured and then laser printing is performed on individual films cut from the roll, printing unevenness, i.e., unevenness in the density of the laser printing, can occur on each film.

[0007] An object of the present invention is to provide pellets that can be used to produce molded articles (e.g., containers and films) that can reduce printing unevenness that can occur when laser marking is performed. Another object of the present invention is to provide a method for producing a molded article that can reduce printing unevenness that can occur when laser marking is performed. Another object of the present invention is to provide a film that can reduce printing unevenness that can occur when laser marking is performed.

[0008] In order to solve this problem, the present invention has the following configuration [1]: [1] A pellet containing a polyolefin and a laser marking agent, the pellet having an angle of repose of 25 degrees or more and 45 degrees or less.

[0009] According to [1], since the pellets contain a laser marking agent, it is possible to produce a molded product on which a mark can be formed by a laser, that is, a laser-markable molded product.

[0010] Furthermore, since the angle of repose of the pellets is 25 degrees or more and 45 degrees or less, molded articles with reduced printing unevenness can be produced. This will be explained below. Since the angle of repose of the pellets is 25 degrees or more and 45 degrees or less, when the pellets of the present invention (i.e., the pellets according to [1]) are mixed with other pellets (e.g., second pellets) and then fed from a hopper to an extruder, it is possible to reduce the variation over time in the amount of the pellets of the present invention (i.e., the pellets according to [1]) fed per unit time, and it is possible to reduce the variation over time in the concentration of the laser marking agent in the molten material in the extruder. Therefore, it is possible to reduce the variation in the concentration of the laser marking agent in the molded article, and it is possible to reduce printing unevenness that may occur when laser marking is performed on the molded article. For example, when the molded article is a roll-shaped film produced through a process of extruding a film-shaped molten material, it is possible to reduce the variation in the concentration of the laser marking agent in the length direction of the film. Therefore, when laser marking is performed on a film cut from the roll, it is possible to reduce printing unevenness that may occur from film to film. On the other hand, when the molded product is a container manufactured by blow molding a parison containing a layer extruded by an extruder, it is possible to reduce printing unevenness that can occur between containers.

[0011] The present invention preferably has the following configurations [2] to [4]. [2] The pellet according to [1], wherein the content of the laser marking agent is 1% by mass or more and 50% by mass or less. [3] The pellet according to [1] or [2], wherein the weight per pellet is 8 mg or more and 20 mg or less. [4] The pellet according to any of [1] to [3], which is used to manufacture a container.

[0012] The present invention has the following configuration [5]. [5] A method for producing a molded product, comprising: a step of mixing at least the pellet according to any one of [1] to [4] and a second pellet; a step of supplying the mixed pellets prepared in the step of mixing at least the pellet and the second pellet from a hopper to an extruder; and a step of melting and extruding the mixed pellets in the extruder.

[0013] The present invention preferably has the following configurations [6] to [8]. [6] The method for producing a molded article according to [5], further comprising a step of blow molding a parison including a layer extruded by the extruder. [7] The method for producing a molded article according to [5], wherein the step of melting and extruding the mixed pellets in the extruder extrudes a film-like melt. [8] The method for producing a molded article according to any one of [5] to [7], wherein the difference in the angle of repose of the pellet and the angle of repose of the second pellet is 10 degrees or less in absolute value.

[0014] The present invention has the following configuration [9]. [9] A film comprising a polyolefin and a laser marking agent, wherein the content of a major metal element in the laser marking agent varies by 0.10 mass% or less in the longitudinal direction of the film, and the variation is the absolute value of the difference between the average value of the content of the major metal element measured at 50 m intervals in the longitudinal direction of the film and the value farthest from the average value. Here, "the major metal element in the laser marking agent" means the metal element that is contained in the largest amount among the metal elements contained in the laser marking agent.

[0015] According to [9], the fluctuation range of the content of the main metal elements in the laser marking agent in the longitudinal direction of the film is 0.10 mass% or less, so that it is possible to reduce printing unevenness that may occur when laser marking is performed.

[0016] According to the present invention, it is possible to provide pellets that can be used to produce molded articles (for example, containers and films) that can reduce printing unevenness that can occur when laser marking is performed. According to the present invention, it is also possible to provide a method for producing a molded article that can reduce printing unevenness that can occur when laser marking is performed. According to the present invention, it is also possible to provide a film that can reduce printing unevenness that can occur when laser marking is performed.

[0017] 1A and 1B are schematic perspective views for explaining the measured lengths of pellets in the shape of an elliptical cylinder and an ellipsoid, respectively.

[0018] Hereinafter, embodiments of the present invention will be described in detail.

[0019] <1. Pellets> <1.1. Polyolefin> The pellets of this embodiment contain a polyolefin. The polyolefin may be a homopolymer or a copolymer. Examples of polyolefins include polyethylenes such as low-density polyethylene (LDPE), high-density polyethylene (HDPE), and linear low-density polyethylene (LLDPE). In addition, examples of polyolefins include homopolypropylene and ethylene-propylene copolymers. Examples of polyolefins include olefin-based thermoplastic elastomers and ionomers. The polyolefin may have a functional group. Examples of functional groups include amino groups, isocyanate groups, hydroxyl groups, mercapto groups, ureido groups, glycidyl groups, carboxylic acid groups, carboxylic anhydride groups, carboxylic acid ester groups, and metal carboxylate groups. Examples of polyolefins having functional groups include Admer (registered trademark), an adhesive polyolefin from Mitsui Chemicals, Inc. Note that one type of polyolefin may be used, or two or more types may be used.

[0020] 1.2 Laser Marking Agent The pellets of this embodiment contain a laser marking agent. Because the pellets contain a laser marking agent, it is possible to produce a molded article on which a mark can be formed by a laser, that is, a laser-markable molded article.

[0021] The laser marking agent can be a pigment capable of absorbing a laser. If the laser marking agent can absorb a laser, it can convert the laser energy into heat, thereby carbonizing the surrounding polyolefin. Of course, the laser marking agent itself may be capable of changing color (for example, changing color to black). In this way, the laser marking agent may be capable of carbonizing the surrounding polyolefin, or may be capable of changing color itself, or may be capable of both.

[0022] As a laser, for example, CO 2 Laser (10600 nm), YAG laser (1064 nm), YVO 4 Laser (1064 nm), fiber laser (1090 nm), green laser (532 nm), ultraviolet laser (hereinafter sometimes referred to as "UV laser") (355 nm) are examples of such lasers. 4 Laser, fiber laser, green laser, and UV laser are preferred, and Nd:YAG laser, fiber laser, green laser, and UV laser are more preferred.

[0023] The laser marking agent may contain, for example, at least one elemental metal selected from the group consisting of bismuth, gadolinium, neodymium, titanium, antimony, tin, and aluminum, and / or at least one oxide of a metal selected from this group. Of course, the laser marking agent may also contain elemental metals or oxides of metals other than these.

[0024] The particle size of the laser marking agent is preferably 0.1 μm or more, more preferably 0.5 μm or more, while the particle size of the laser marking agent is preferably 10 μm or less, more preferably 9 μm or less.

[0025] Commercially available laser marking agents include, for example, "TOMATEC COLOR" from TOMATEC Corporation and "Iriotec (registered trademark)" from Merck Performance Materials LLC. One type of laser marking agent may be used, or two or more types may be used.

[0026] The content of the laser marking agent in the pellets is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more. The content of the laser marking agent may be 10% by mass or more, 15% by mass or more, or even 20% by mass or more. On the other hand, the content of the laser marking agent in the pellets is preferably 50% by mass or less, more preferably 35% by mass or less, even more preferably 30% by mass or less, and even more preferably 25% by mass or less. When it is 50% by mass or less, the true specific gravity of the pellets can be prevented from becoming excessively high. The content of the laser marking agent may be 40% by mass or less, 30% by mass or less, or 25% by mass or less.

[0027] 1.3. Physical Properties and Weight of Pellets> The angle of repose of the pellets is 25 degrees or more and 45 degrees or less. By setting the angle of repose at 25 degrees or more and 45 degrees or less, molded articles with reduced printing unevenness can be produced. This will be explained below. Because the angle of repose of the pellets is 25 degrees or more and 45 degrees or less, when the pellets of this embodiment are mixed with other pellets and then fed from a hopper to an extruder, it is possible to reduce the variation over time in the amount of pellets of this embodiment fed per unit time, and it is possible to reduce the variation over time in the concentration of the laser marking agent in the molten material in the extruder. Therefore, it is possible to reduce the variation in the concentration of the laser marking agent in the molded article, and it is possible to reduce printing unevenness that may occur when laser marking is performed on the molded article. For example, when the molded article is a roll-shaped film produced through a process of extruding a film-shaped molten material, it is possible to reduce the variation in the concentration of the laser marking agent in the length direction of the film. Therefore, when laser marking is performed on a film cut from the roll, it is possible to reduce printing unevenness that may occur from film to film. On the other hand, when the molded product is a container manufactured by blow molding a parison including layers extruded by an extruder, printing unevenness that may occur in each container can be reduced. The angle of repose of the pellets is preferably 28 degrees or more, more preferably 30 degrees or more, and even more preferably 32 degrees or more. On the other hand, the angle of repose of the pellets is preferably 43 degrees or less, and more preferably 42 degrees or less.

[0028] Examples of the shape of the pellets include a cylindrical shape such as a right circular cylinder or an elliptical cylinder, and an ellipsoid shape. When the pellets have such a shape, the height of the pellets may be, for example, 1.0 mm or more, 1.3 mm or more, or 1.5 mm or more. On the other hand, the height of the pellets may be, for example, 10.0 mm or less, 7.0 mm or less, or 5.0 mm or less.

[0029] The weight per pellet is preferably 8 mg or more and 20 mg or less. The weight per pellet may be, for example, 9 mg or more, or 10 mg or more. On the other hand, the weight per pellet may be, for example, 18 mg or less, 17 mg or less, or 16 mg or less.

[0030] The bulk density of the pellets is, for example, 0.30 g / cm 3 or more, and 0.40 g / cm 3 or more, and 0.45 g / cm 3 or more, and 0.50 g / cm 3 or more, and 0.52 g / cm 3 or more, and 0.54 g / cm 3 On the other hand, the bulk density of the pellets may be, for example, 0.60 g / cm 3 or less, 0.57 g / cm 3 or less, and 0.55 g / cm 3 It may be the following:

[0031] The true specific gravity of the pellet is, for example, 0.94 g / cm 3 or more, and 1.00 g / cm 3 or more, and 1.02 g / cm 3 or more, and 1.03 g / cm 3 On the other hand, the true specific gravity of the pellets may be, for example, 1.20 g / cm 3 or less, 1.15 g / cm 3 or less, 1.12 g / cm 3or less, 1.10 g / cm 3 It may be the following:

[0032] 2. Method for Producing Molded Article The method for producing a molded article of the present embodiment includes at least a step of mixing the above-mentioned pellets (i.e., pellets containing a polyolefin and a laser marking agent and having an angle of repose of 25 degrees or more and 45 degrees or less; hereinafter, sometimes referred to as "first pellets") and second pellets (hereinafter, sometimes referred to as "mixing step"); a step of supplying the mixed pellets prepared in the step of mixing at least the first pellets and the second pellets from a hopper to an extruder (hereinafter, sometimes referred to as "supply step"); and a step of melting the mixed pellets in the extruder and extruding them (hereinafter, sometimes referred to as "extrusion step").

[0033] Examples of molded articles produced by the manufacturing method of this embodiment include containers and films. Examples of molded articles include parisons.

[0034] Examples of containers include containers for foods and beverages, medicines, quasi-drugs, cosmetics, dentifrice, paints, and adhesives. Examples of foods and beverages include mayonnaise, ketchup, wasabi paste, mustard paste, and pizza sauce. Of these, containers for foods and beverages are preferred, and containers for sauces such as mayonnaise and ketchup are more preferred.

[0035] On the other hand, the film can be used as, for example, a label or a container lid. The film can also be used to produce labels, container lids, bags, laminated tubes, etc. Examples of labels include bottle labels. Examples of bags include bags made by heat sealing, such as vertical pillow bags, horizontal pillow bags, and gusset bags. Examples of bags made by fusion sealing can also be mentioned.

[0036] The following describes a method for manufacturing a container and a method for manufacturing a film.

[0037] 2.1. Method for Manufacturing Container The method for manufacturing a container of this embodiment includes at least a step of mixing first pellets (i.e., pellets containing a polyolefin and a laser marking agent and having an angle of repose of 25 degrees or more and 45 degrees or less) and second pellets (i.e., a mixing step), a step of supplying the mixed pellets prepared in the step of mixing at least the first pellets and the second pellets from a hopper to an extruder (i.e., a supply step), a step of melting and extruding the mixed pellets in the extruder (i.e., an extrusion step), and a step of blow-molding a parison including the layer extruded by the extruder (hereinafter, this may be referred to as a "blow-molding step").

[0038] <2.1.1. Mixing Step> In the mixing step, the first pellets and the second pellets are mixed. Mixing can be performed, for example, by a mixer provided upstream of a hopper. In this case, after mixing, the mixed pellets are transferred from the mixer to the hopper. A feeder may be provided between the mixer and the hopper. Alternatively, mixing may be performed within the hopper.

[0039] The second pellets preferably contain a polyolefin. The description of the polyolefin of the second pellets overlaps with the above description (i.e., the description of the polyolefin of the first pellets), so it will be omitted. Therefore, the description of the polyolefin of the first pellets can also be used as the description of the polyolefin of the second pellets.

[0040] When the polyolefin of the first pellets contains polyethylene, it is preferable that the polyolefin of the second pellets also contains polyethylene. For example, when the polyolefin of the first pellets contains low-density polyethylene, it is preferable that the polyolefin of the second pellets also contains low-density polyethylene. When the polyolefin of the first pellets contains linear low-density polyethylene, it is preferable that the polyolefin of the second pellets also contains linear low-density polyethylene. On the other hand, when the polyolefin of the first pellets contains polypropylene, it is preferable that the polyolefin of the second pellets also contains polypropylene.

[0041] The second pellets may or may not contain a laser marking agent, but it is preferred that the second pellets do not contain a laser marking agent, because since the first pellets contain a laser marking agent, the second pellets do not need to contain a laser marking agent.

[0042] The angle of repose of the second pellets is preferably 15 degrees or more and 55 degrees or less. When the angle is 15 degrees or more and 55 degrees or less, it is possible to prevent the ease with which the second pellets fall from the hopper from deviating excessively from that of the first pellets (i.e., the ease with which they fall), and therefore, it is possible to further suppress the variation over time in the amount of first pellets supplied per unit time. As a result, it is possible to further reduce printing unevenness that may occur when laser printing is performed on a molded product, i.e., a container. The angle of repose of the second pellets is more preferably 20 degrees or more, even more preferably 25 degrees or more, even more preferably 28 degrees or more, even more preferably 30 degrees or more, and even more preferably 32 degrees or more. On the other hand, the angle of repose of the second pellets is more preferably 43 degrees or less, even more preferably 41 degrees or less, and even more preferably 40 degrees or less.

[0043] The description of the shape, weight (specifically, the weight per second pellet), and bulk specific gravity of the second pellets will be omitted because they overlap with the above description (i.e., the description of these for the first pellets). Therefore, the description of the shape, weight, and bulk specific gravity of the first pellets can also be used as the description of these for the second pellets.

[0044] The difference between the angle of repose of the first pellets and the angle of repose of the second pellets is preferably 10 degrees or less in absolute value, more preferably 9 degrees or less, even more preferably 8 degrees or less, even more preferably 7 degrees or less, and even more preferably 6 degrees or less. When the angle of repose is 10 degrees or less, it is possible to prevent the ease with which the first pellets fall from the hopper from deviating excessively from that of the second pellets (i.e., the ease with which they fall), thereby further suppressing the variation over time in the amount of first pellets supplied per unit time. As a result, it is possible to further reduce printing unevenness that may occur when laser marking is performed on a molded product, i.e., a container. This difference may be 5 degrees or less in absolute value, 4 degrees or less in absolute value, 3 degrees or less in absolute value, or 2 degrees or less in absolute value.

[0045] In the mixing step, other pellets (e.g., third pellets) may be further mixed with the first and second pellets. The description of the other pellets overlaps with the description of the second pellets, so they will be omitted. Therefore, the description of the second pellet can also be used as a description of the other pellets.

[0046] The difference between the maximum and minimum angles of repose of the individual pellets mixed in the mixing step (i.e., the first pellets, the second pellets, and other pellets mixed as needed) is preferably 10 degrees or less, more preferably 9 degrees or less, even more preferably 8 degrees or less, even more preferably 7 degrees or less, and even more preferably 6 degrees or less. If the angle is 10 degrees or less, it is possible to further reduce the variation over time in the amount of first pellets supplied per unit time, thereby further reducing printing unevenness that may occur when laser printing is performed on the container. This difference may be 5 degrees or less in absolute value, or may be 4 degrees or less in absolute value.

[0047] The amount of the first pellets is preferably 1.0% by mass or more, more preferably 1.5% by mass or more, of the total mass (100% by mass) of the pellets mixed in the mixing step (i.e., the first pellets, the second pellets, and other pellets mixed as needed). The amount of the first pellets may be 3.0% by mass or more, or even 5.0% by mass or more. On the other hand, the amount of the first pellets is preferably 50% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less, of the total mass (100% by mass) of the pellets mixed in the mixing step.

[0048] Of the total mass (100% by mass) of pellets mixed in the mixing step (i.e., first pellets, second pellets, and other pellets mixed as needed), the amount of second pellets is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, and even more preferably 60% by mass or more. On the other hand, of the total mass (100% by mass) of pellets mixed in the mixing step, the amount of second pellets is preferably 99.0% by mass or less, more preferably 98.5% by mass or less, and even more preferably 97.0% by mass or less.

[0049] 2.1.2. Feeding Step In the feeding step, the mixed pellets are fed from a hopper to the extruder. The hopper may be provided above the feed port of the extruder. The hopper is funnel-shaped. The hopper may be provided with a device for promoting the discharge of the mixed pellets, such as a vibrator, an air knocker, or a screw.

[0050] The inclination angle of the hopper may be, for example, 40 degrees or more, 45 degrees or more, or 50 degrees or more. On the other hand, the inclination angle of the hopper may be, for example, 75 degrees or less, or 70 degrees or less. The inclination angle of the hopper is the angle formed by a pair of opposing inner surfaces of the hopper. For example, if the hopper has a taper, i.e., a conical portion, the inclination angle is the angle formed by a pair of opposing inner surfaces of the hopper in a cross-sectional view when the hopper is assumed to be cut along a plane perpendicular to the diameter of the conical portion and located at the center of the diameter. Note that if the inclination angle varies depending on the measurement location, the "inclination angle of the hopper" is expressed as the minimum value.

[0051] 2.1.3. Extrusion Process In the extrusion process, the mixed pellets are melted and extruded in an extruder to form a parison.

[0052] The extruder includes a screw and a cylinder surrounding the screw. That is, the extruder includes a cylinder and a screw inside the cylinder. The extruder can melt the mixed pellets by the rotating screw and extrude them at a fixed amount. Examples of the extruder include a single-screw extruder and a twin-screw extruder.

[0053] The extruder is equipped with a die, which may be attached to the cylinder via a head (i.e., extruder head), or the die may include the head.

[0054] Specifically, in the extrusion process, the mixed pellets are melted in an extruder, and the melted mixed pellets are layered with melts from other extruders as needed, and then the melt, i.e., the parison, is extruded through a die. These melts can be layered in the head or the die. The number of other extruders may be one or more.

[0055] Examples of the resin supplied to the other extruder include polyamide, ethylene-vinyl alcohol copolymer (EVOH), and polyolefin. The resin supplied to the other extruder may be in pellet form. An example of polyamide is polymetaxylylene adipamide (MXD6). The description of polyolefins overlaps with the above description (i.e., the description of the polyolefins of the first pellets), so they will be omitted. Therefore, the description of the polyolefins of the first pellets can also be used as a description of the polyolefins supplied to the other extruders.

[0056] 2.1.4. Blow Molding Process In the blow molding process, a parison is blown. For example, compressed gas (e.g., compressed air) is blown into the parison, and the parison is pressed against the inner surface of a mold. This produces a hollow molded product, specifically a container. Note that the blow molding may be, for example, direct blow molding (i.e., extrusion blow molding) or injection blow molding.

[0057] The parison includes a layer (hereinafter sometimes referred to as the "laser-markable layer") formed using the mixed pellets as a raw material. The laser-markable layer includes a polyolefin and a laser-marking agent. The laser-markable layer may further include various additives. Examples of additives include waxes, antioxidants, antistatic agents, crystal nucleating agents, viscosity reducers, heat stabilizers, coloring pigments, color inhibitors, UV absorbers, and lubricants.

[0058] The parison may consist of only the laser marking layer, i.e., it may be a single layer, or it may include multiple layers.

[0059] When the parison includes multiple layers, the parison may further include a layer containing an ethylene-vinyl alcohol copolymer (i.e., EVOH). When the parison includes a layer containing an ethylene-vinyl alcohol copolymer, the gas barrier properties of the container can be improved. The parison may also include a layer containing a polyolefin (e.g., a polyolefin having a functional group) between the layer containing the ethylene-vinyl alcohol copolymer and the laser-markable layer.

[0060] When the parison includes multiple layers, the following layer configurations can be mentioned, for example. In the following, a layer containing polyethylene may be referred to as a "polyethylene layer," a layer containing an ethylene-vinyl alcohol copolymer as an "EVOH layer," and a layer containing an adhesive resin (for example, a polyolefin having a functional group) as an "adhesive resin layer." Polyethylene layer / laser marking layer / adhesive resin layer / EVOH layer / adhesive resin layer / polyethylene layer Polyethylene layer / EVOH layer / adhesive resin layer / laser marking layer / adhesive resin layer / EVOH layer / polyethylene layer

[0061] A container can be obtained by the above procedure. The container may be subjected to some processing as needed.

[0062] 2.2. Film Manufacturing Method The film manufacturing method of the present embodiment includes at least a step of mixing first pellets (i.e., pellets containing a polyolefin and a laser marking agent and having an angle of repose of 25 degrees or more and 45 degrees or less) and second pellets (i.e., a mixing step), a step of supplying the mixed pellets prepared in the step of mixing at least the first pellets and the second pellets from a hopper to an extruder (i.e., a supply step), a step of melting and extruding the mixed pellets in the extruder (i.e., an extrusion step), and a step of solidifying the film-like molten material including the layer extruded in the extruder with a chill roll.

[0063] 2.2.1 Mixing Step and Supply Step The description of the mixing step and supply step in the film manufacturing method of this embodiment overlaps with the above description (i.e., the description of the mixing step and supply step in the container manufacturing method), so will be omitted. Therefore, the description of the mixing step and supply step in the container manufacturing method can also be used as the description of the mixing step and supply step in the film manufacturing method.

[0064] 2.2.2. Extrusion Step In the extrusion step, the mixed pellets are melted in an extruder, and the melt is extruded from a die in the form of a film.

[0065] The extruder includes a screw and a cylinder surrounding the screw. That is, the extruder includes a cylinder and a screw inside the cylinder. The extruder can melt the mixed pellets by the rotating screw and extrude them at a fixed amount. Examples of the extruder include a single-screw extruder and a twin-screw extruder.

[0066] The extruder is equipped with a die, which may be attached to the cylinder via a head (i.e., extruder head), or the die may include the head.

[0067] In the extrusion process, specifically, the mixed pellets are melted in an extruder, and the melted mixed pellets are optionally laminated with melts from other extruders, and the resulting film-like melt is extruded through a die. These melts can be laminated in a feed block or a die. The number of other extruders may be one or more.

[0068] The resins supplied to the other extruders will not be described here because they overlap with the above description (i.e., the description of the resins in the container manufacturing method). Therefore, the description of the resins in the container manufacturing method can also be used as the description of the resins in the film manufacturing method.

[0069] <2.2.3. Other Steps> The film-like molten material is solidified with a chill roll. This allows the film-like molten material to be rapidly cooled and solidified, resulting in a substantially unoriented film (hereinafter sometimes referred to as an "unstretched film"). The surface temperature of the chill roll is preferably 40°C or less.

[0070] The unstretched film can then be stretched. For example, it can be biaxially stretched. The biaxial stretching may be simultaneous biaxial stretching or sequential biaxial stretching. Of these, sequential biaxial stretching is preferred. In sequential biaxial stretching, it is preferred to stretch the unstretched film in the longitudinal direction (MD), and then stretch the sheet after MD stretching in the width direction (TD).

[0071] The method for stretching the unstretched film in the longitudinal direction may be, for example, a method of stretching in multiple stages between a plurality of rolls, or a method of stretching while heating with an infrared heater, etc. Of these, the former is preferred.

[0072] When stretching in the longitudinal direction, it is preferable to preheat the unstretched film so that its temperature is 100° C. to 180° C. If the temperature is 100° C. or higher, breakage that may occur when the unstretched film is stretched in the longitudinal direction can be suppressed.

[0073] The stretching ratio when stretching the preheated unstretched film in the longitudinal direction, i.e., the MD stretching ratio, is preferably 1.1 times or more, more preferably 1.5 times or more, and even more preferably 2.0 times or more. If it is 1.1 times or more, it is possible to impart molecular orientation to the film in the longitudinal direction, thereby improving the mechanical strength. The MD stretching ratio is preferably 10 times or less, more preferably 9.5 times or less, and even more preferably 9.0 times or less. If it is 10 times or less, it is possible to suppress breakage that may occur during TD stretching.

[0074] At least one surface of the longitudinally stretched film may be subjected to a surface treatment such as a corona treatment or a plasma treatment, if necessary. At least one surface of the longitudinally stretched film may be coated with a resin dispersion or a resin solution, if necessary.

[0075] The film stretched in the longitudinal direction is introduced into a tenter device, both ends of the film are held with clips, the film is heated with hot air, and then the distance between the clips, i.e., the gap, is increased while the film is transported in the longitudinal direction, thereby stretching the film in the width direction.

[0076] The preheating temperature when stretching the film in the width direction is preferably 110° C. or higher and 170° C. or lower. The temperature when stretching the film in the width direction, i.e., the TD stretching temperature, is preferably 120° C. or higher and 180° C. or lower.

[0077] The stretching ratio when stretching the film in the width direction, i.e., the TD stretching ratio, is preferably 1.5 times or more, more preferably 2.0 times or more, and is preferably 20 times or less, more preferably 15 times or less.

[0078] A film stretched in the width direction, i.e., a biaxially stretched film, can be introduced into a zone for heat treatment (hereinafter, sometimes referred to as a "heat treatment zone"). Before being introduced into the heat treatment zone, the biaxially stretched film may be introduced into a zone where active heating is not performed (hereinafter, sometimes referred to as an "intermediate zone"). In other words, the biaxially stretched film may be introduced into the intermediate zone before being introduced into the heat treatment zone.

[0079] In the heat treatment zone, the film is preferably heated to a temperature of 130°C or higher and 190°C or lower. Heat treatment promotes crystallization of the film, making it easier to reduce the heat shrinkage rate. The heating temperature is preferably 135°C or higher. On the other hand, the heating temperature is preferably 185°C or lower, and more preferably 180°C or lower.

[0080] During the heat treatment, the distance between the clips of the tenter may be reduced, thereby reducing the thermal shrinkage rate in the width direction.

[0081] The film that has passed through the heat treatment zone can be guided to a cooling zone, where it is preferably cooled with cooling air at 10° C. to 30° C. for 2 to 20 seconds.

[0082] The film can be wound up while cutting and removing both ends as needed. Slitting can also be performed as needed before winding. A roll-shaped film can be obtained by this procedure. Printing can be performed at any time, and the gas barrier layer can be formed at any time. Examples of raw materials for the gas barrier layer include metals such as silicon, aluminum, tin, zinc, iron, and manganese, and inorganic compounds containing one or more of these metals. Examples of inorganic compounds include oxides, nitrides, carbides, and fluorides.

[0083] 2.2.4. Film The film includes a layer (i.e., a laser-markable layer) formed using the mixed pellets as a raw material. The laser-markable layer includes a polyolefin and a laser-marking agent. The laser-markable layer may further include various additives. Examples of additives include waxes, antioxidants, antistatic agents, crystal nucleating agents, viscosity reducers, heat stabilizers, coloring pigments, color inhibitors, UV absorbers, and lubricants.

[0084] The thickness of the laser marking layer is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more. The thicker the thickness, the darker the mark formed by the laser, i.e., the laser marking, can be. On the other hand, the thickness of the laser marking layer is preferably 100 μm or less, more preferably 95 μm or less, and even more preferably 90 μm or less. The thinner the thickness, the more the haze of the film tends to be reduced.

[0085] The film may consist of only the laser marking layer, i.e., it may be a single layer.

[0086] On the other hand, the film may include a laser marking layer and other layers. That is, the film may include multiple layers. For example, the film may include a first layer, a second layer, and a third layer. The first layer, the second layer, and the third layer are arranged in this order in the thickness direction of the film. Here, at least one of the first layer, the second layer, and the third layer may be a laser marking layer. Note that other layers may exist between the first layer and the second layer, or between the second layer and the third layer.

[0087] When the film includes a first layer, a second layer, and a third layer, and the second layer is the laser-markable layer, the first layer preferably contains a polyolefin. The description of the polyolefin in the first layer overlaps with the above description (i.e., the description of the polyolefin in the first pellets), so it is omitted here. Therefore, the description of the polyolefin in the first pellets can also be used as the description of the polyolefin in the first layer. When the polyolefin in the laser-markable layer contains polyethylene, it is preferable that the first layer also contains polyethylene. For example, when the laser-markable layer contains low-density polyethylene, it is preferable that the first layer also contains at least one of low-density polyethylene and high-density polyethylene. When the laser-markable layer contains linear low-density polyethylene, it is preferable that the first layer also contains linear low-density polyethylene. On the other hand, when the laser-markable layer contains polypropylene, it is preferable that the first layer also contains polypropylene.

[0088] The first layer preferably further contains a lubricant. Examples of the lubricant include particles such as silica and talc. Examples of the lubricant include fatty acid amides, alkyl sulfonates, stearic acids, and erucic acid amides. The first layer may also contain various additives.

[0089] When the film includes a first layer, a second layer, and a third layer, and the second layer is the laser-markable layer, the third layer preferably contains a polyolefin. The description of the polyolefin of the third layer overlaps with the above description (i.e., the description of the polyolefin of the first pellets), so it is omitted here. Therefore, the description of the polyolefin of the first pellets can also be used as the description of the polyolefin of the third layer. When the polyolefin of the laser-markable layer contains polyethylene, it is preferable that the third layer also contains polyethylene. For example, when the laser-markable layer contains low-density polyethylene, it is preferable that the third layer also contains at least one of low-density polyethylene and high-density polyethylene. When the laser-markable layer contains linear low-density polyethylene, it is preferable that the third layer also contains linear low-density polyethylene. On the other hand, when the laser-markable layer contains polypropylene, it is preferable that the third layer also contains polypropylene.

[0090] The third layer preferably further contains a lubricant. Examples of the lubricant include particles such as silica and talc. Examples of the lubricant include fatty acid amides, alkyl sulfonates, stearic acids, and erucic acid amides. The third layer may also contain various additives.

[0091] The film may be subjected to corona treatment, coating treatment, flame treatment, or the like.

[0092] The thickness of the film is preferably 8 μm or more, more preferably 13 μm or more, and even more preferably 18 μm or more. The thickness of the film may be, for example, 20 μm or more, or may be 30 μm or more. On the other hand, the thickness of the film is preferably 200 μm or less, more preferably 195 μm or less, and even more preferably 190 μm or less. The thinner the thickness, the more cost can be reduced. The thickness of the film may be, for example, 150 μm or less, 100 μm or less, 80 μm or less, or 60 μm or less.

[0093] When the film is in a roll form, the length of the film may be, for example, 500 m or more, 1000 m or more, 5000 m or more, or 10000 m or more.

[0094] In the longitudinal direction of the film, the content of the major metal element of the laser marking agent (hereinafter sometimes referred to as the "major metal element of the laser marking agent") preferably fluctuates by 0.10% by mass or less, more preferably by 0.09% by mass or less, even more preferably by 0.08% by mass or less, and even more preferably by 0.07% by mass or less. Here, "major metal element of the laser marking agent" refers to the metal element with the highest content among the metal elements contained in the laser marking agent. The major metal element of the laser marking agent preferably accounts for 50% by mass or more when the content of all metal elements in the laser marking agent is taken as 100% by mass. Note that the major metal element of the laser marking agent may account for 50% by mass or more when the content of all metal elements in the film is taken as 100% by mass. Examples of major metal elements of the laser marking agent include Sn (tin), Bi (bismuth), Ti (titanium), Nd (neodymium), Gd (gadolinium), Sb (antimony), Al (aluminum), and Mo (molybdenum). For example, the main metal element of IRIOTEC (registered trademark) 8825 (Merck Performance Materials, main component: antimony-doped tin / mica) used in the examples described later is Sn, i.e., tin. On the other hand, TOMATEC COLOR 42-920A (TOMATEC Corporation, main component: Bi) 2 O 3The main metal element of the laser marking agent is Bi, i.e., bismuth. The fluctuation range of the content of the main metal element of the laser marking agent is the absolute value of the difference between the average value when the content of the main metal element of the laser marking agent is measured at 50 m intervals along the length of the film and the value farthest from the average value. This fluctuation range can be determined by the method described in the Examples. If the fluctuation range is 0.10% by mass or less, it is possible to reduce printing unevenness that may occur when laser marking is performed. The fluctuation range may be, for example, 0.001% by mass or more, 0.003% by mass or more, 0.005% by mass or more, 0.01% by mass or more, or 0.02% by mass or more.

[0095] Laser marking L in the length direction of the film * The variation in the value is preferably 2.5 or less, more preferably 2.0 or less, even more preferably 1.7 or less, and even more preferably 1.5 or less. * The variation in value is determined by laser marking at 50m intervals along the length of the film, and then measuring the L of the laser marking. * value (i.e., L of the laser-irradiated part) * The variation is the difference between the maximum and minimum values ​​when the saturation value (value) is measured. This variation can be determined by the method described in the Examples.

[0096] The present invention will be described in more detail below with reference to examples and comparative examples. Unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".

[0097] <1. Raw Materials> The following raw materials were used. <1.1. Polyolefins> Sumitomo Noblen (registered trademark) FS2011DG3 (polypropylene manufactured by Sumitomo Chemical Co., Ltd.) Novatec PP FL203D (polypropylene manufactured by Japan Polypropylene Corporation) Sumikathene (registered trademark) FV405 (linear low-density polyethylene manufactured by Sumitomo Chemical Co., Ltd.) Harmolex NC564A (linear low-density polyethylene manufactured by Japan Polyethylene Corporation) Sumikathene (registered trademark) FV407 (linear low-density polyethylene manufactured by Sumitomo Chemical Co., Ltd.) Hi-Zex (HZ) 2300L (high-density polyethylene manufactured by Prime Polymer Co., Ltd.)

[0098] The size, true specific gravity, bulk specific gravity, weight (specifically, weight per particle), and angle of repose of these particles were measured. The measurement methods will be described later. The results are shown in Table 1. In Table 1, "-" indicates that the measurement or evaluation was not performed.

[0099] <1.2. Laser marking agent> IRIOTEC (registered trademark) 8825 (Merck Performance Materials, main component: antimony-doped tin / mica) TOMATEC COLOR 42-920A (TOMATEC Corporation, main component: Bi 2 O 3 )

[0100] <2. Production of Masterbatch Pellets> <2.1. Production of Pellets B, J, L, and M> FS2011DG3 and IRIOTEC (registered trademark) 8825 were mixed (dry blended) in a mass ratio of 80:20, charged into a twin-screw extruder, and melted and mixed at 250°C. A cylindrical strand was discharged from a strand die, cooled with water, and cut with a strand cutter to obtain Pellets B. Pellets J, L, and M were obtained using the same procedure as for Pellets B, except that the raw materials were mixed as described in Table 2.

[0101] 2.2. Preparation of Pellets E and K FV405 and IRIOTEC (registered trademark) 8825 were mixed (dry blended) in a mass ratio of 90:10, charged into a twin-screw extruder, and melted and mixed at 250°C. A cylindrical strand was discharged from a strand die, cooled with water, and cut with a strand cutter to obtain Pellets E. Pellets K were obtained using the same procedure as for Pellets E, except that the raw materials were mixed as described in Table 2.

[0102] 2.3. Preparation of Pellet F FV405 and silica were mixed so that the silica concentration was 20,000 ppm, and the mixture was charged into a twin-screw extruder and melted and mixed at 250° C. A cylindrical strand was discharged from a strand die, cooled with water, and cut with a strand cutter to obtain pellet F.

[0103] 2.4. Measurement results of masterbatch pellets The size, true specific gravity, bulk specific gravity, weight (specifically, weight per pellet), and angle of repose of the masterbatch pellets were measured. The measurement methods will be described later. The results are shown in Table 2. In addition, "-" in the row for laser marking agent means that no laser marking agent was added. Also in the row for lubricant, "-" means that no lubricant was added. The shape, size, true specific gravity, bulk specific gravity, and weight per pellet of pellet F were not measured.

[0104] <3. Film Production> <3.1. Film Production in Example 1> Pellets B and pellets C were mixed in a mass ratio of 1.5:98.5 and then fed from a hopper (inclination angle 60°) into a single-screw extruder. The mixture was melted at 250°C and extruded into a film-like melt from a T-die. The film-like melt was cooled and solidified on a chill roll set at a surface temperature of 30°C. This resulted in an unstretched film. The unstretched film was introduced into a longitudinal stretching machine with multiple roll groups arranged in series, preheated on a preheated roll until the film temperature reached 125°C, and then stretched 4.5 times. The longitudinally stretched film was introduced into a transverse stretching machine (i.e., tenter) and preheated for 5 seconds until the surface temperature reached 160°C, after which it was stretched 9 times in the width direction (transverse direction). The film was then introduced into a heat treatment zone and heat-treated at 163°C for 5 seconds. At this time, a 7% relaxation treatment was performed in the width direction. After passing through the heat treatment zone, the film was cooled for 5 seconds with cooling air at 30°C, and then both edges of the film were cut off and wound into a roll having a width of 400 mm and a thickness of 40 µm, thereby obtaining a film having a length of 500 m.

[0105] 3.2. Preparation of Films in Examples 3 and 4 and Comparative Examples 2 and 3 Films were obtained in the same manner as in Example 1, except that the pellets were mixed as shown in Table 3.

[0106] 3.3. Preparation of Film in Comparative Example 1 As shown in Table 3, a film was obtained in the same manner as in Example 1, except that only pellets C were used as pellets.

[0107] 3.4. Film Production in Example 2 To obtain the raw material for the core layer, pellets D, E, and G were mixed in a mass ratio of 30:3:67. Meanwhile, to obtain the raw material for the skin layer, pellets F, H, and I were mixed in a mass ratio of 10:80:10. The raw material for the skin layer (i.e., a mixture of pellets F, H, and I) was fed to the first and third extruders and melted at 250°C. The raw material for the core layer (i.e., a mixture of pellets D, E, and G) was fed from a hopper (inclination angle 60°) to the second extruder and melted at 250°C. The melts from each extruder were introduced into a feed block, laminated in a skin layer / core layer / skin layer configuration, and then extruded into a film-like melt from a T-die. The extrusion rate was adjusted so that the thickness ratio of the skin layer / core layer / skin layer was 15 / 70 / 15. The film-like melt was cooled and solidified on a chill roll set at a surface temperature of 30° C. The film that had passed through the chill roll, i.e., the unstretched laminated film, had both edges cut and removed, and a film 400 mm wide and 30 μm thick was wound into a roll, thereby obtaining a film 500 m long.

[0108] <4. Measurement Method> <4.1. Size> Various lengths of the pellets were measured using a vernier caliper. Specifically, when the pellets were elliptical cylindrical, dimensions 1, 2, and 3 were measured according to Figure 1. On the other hand, when the pellets were ellipsoidal, dimensions 1, 2, and 3 were measured according to Figure 2. This measurement was performed on 10 pellets, and the average value was calculated.

[0109] 4.2. Weight per pellet The weight (g) of one pellet was measured using a weighing scale. This measurement was carried out for 10 pellets, and the average value was calculated.

[0110] <4.3. True specific gravity> After determining the volume per grain, the true specific gravity (g / mm 3) was calculated. When the pellets were cylindrical, the volume per pellet was calculated using the following formula: Volume = Height x Major axis x Minor axis x 3.14 That is, according to Figure 1, Volume = Dimension 1 x Dimension 2 x Dimension 3 x 3.14 On the other hand, when the pellets were ellipsoidal, as shown in Figure 2, the volume per pellet was calculated using the following formula: Volume = Dimension 1 x Dimension 2 x Dimension 3 x 4 / 3 x 3.14

[0111] <4.4. Bulk specific gravity> The pellets were placed in a metal cup until it was level, and the weight of the pellets in the cup was determined. This procedure was repeated twice, and the average value was calculated. The average value (i.e., the average weight of the pellets in the cup) was divided by the volume of the cup to determine the bulk specific gravity (g / mm 3 The volume of the cup was determined by filling the cup with water, transferring the water to a measuring cylinder, and then measuring the volume of the water.

[0112] 4.5 Angle of Repose A metal cylindrical container stand with a diameter of 50 mm and a polyethylene funnel with a diameter of 10 mm were prepared. The funnel's opening (i.e., the 10 mm diameter outlet) was positioned 50 mm above the center of the top surface of the stand (i.e., the 50 mm diameter plane), and the pellets in the funnel were dropped. This was continued until the periphery of the stand was overflowing with pellets. The angle of repose, i.e., the angle formed by the slope of the pellets piled up on the stand and the top surface of the stand (i.e., the horizontal plane), was measured with a protractor.

[0113] 4.6. Fluctuation Range of the Content of Major Metal Elements in Laser Marking Agents A 500 m long film was sampled at 50 m intervals. Specifically, samples were cut out from the 500 m long film at positions 50 m, 100 m, 150 m, 200 m, 250 m, 300 m, 350 m, 400 m, and 450 m. For each sample, the content of the major metal elements in the laser marking agent was measured, and the average value (i.e., the average content of the major metal elements) was calculated. The absolute value of the difference between the value farthest from the average value (maximum or minimum value) was calculated as the fluctuation range (i.e., the fluctuation range of the content of the major metal elements in the laser marking agent). The content of the major metal elements was calculated using the following method.

[0114] 50 mg of sample was weighed into a 100 mL quartz Erlenmeyer flask, 3 mL of concentrated sulfuric acid was added, and the mixture was gradually heated on a hot plate. Wet carbonization was then performed until the solution turned black. 30% hydrogen peroxide was then added to the solution until it became colorless and transparent, and the mixture was further heated on a hot plate. After confirming that the color of the solution did not change upon heating, the mixture was allowed to cool to room temperature. The cooled solution, i.e., the decomposed solution, was placed in a 50 mL digitube and adjusted to a constant volume of 50 mL with 10 mL of 6N hydrochloric acid and ultrapure water. This resulted in a pretreatment solution. The pretreatment solution was measured using a high-frequency inductively coupled plasma optical emission spectrometer (SPECTROBLUE, manufactured by Hitachi High-Tech Science Corporation) to quantify the amount of metal elements, specifically the amount of major metal elements. When the sample contained IRIOTEC (registered trademark) 8825, Sn was quantified as the major metal element. On the other hand, when the sample contained TOMATEC COLOR 42-920A, Bi was quantified as the major metal element. The content of the major metal element in the sample was defined as A (ppm = mg / kg), the concentration of the major metal element in the pretreatment solution was defined as B (mg / L), and the concentration of the major metal element in a blank test solution used as a measurement blank (i.e., 10 mL of 6N hydrochloric acid was diluted with ultrapure water to a constant volume of 50 mL) was defined as C (mg / L). The amount of the major metal element in 50 mg of sample was calculated as follows: A = (B - C) x 50 / 50

[0115] <4.7. Laser marking L * Variation in values> A 500 m long film was sampled at 50 m intervals. Specifically, samples were cut out from the 50 m, 100 m, 150 m, 200 m, 250 m, 300 m, 350 m, 400 m, and 450 m positions of the 500 m long film. After laser marking on each sample, the L of the laser marking was * value (i.e., L of the laser-irradiated part) * The L * The value was measured twice for each sample, and the L * The average value of the values ​​was calculated. The difference between the maximum and minimum values ​​of these average values ​​was used as the laser marking L. * It was calculated as the variation in values.

[0116] <4.7.1. Laser marking> Each sample was irradiated with a 355 nm ultraviolet (UV) laser marker (MD-U1000, manufactured by Keyence Corporation) under conditions of laser power 40%, scan speed 1000 mm / sec, pulse frequency 40 kHz, and spot variable -20, thereby printing "ABC123." The size of the characters was 0.8 cm ± 0.2 cm in height and 0.6 cm ± 0.2 cm in width per character (for example, "B").

[0117] <4.7.2.L * Value > Laser-printed L * value (i.e., L of the laser-irradiated part) * The L value was measured using a spectrophotometer (ZE-6000, manufactured by Nippon Denshoku Co., Ltd.) by the reflection method. Specifically, the measurement was performed using the following procedure. First, a 3 cm square sample was cut out so that all of the "B" characters in the printed "ABC123" would fit inside. Next, the sample was placed in the opening of a 6 mm diameter sample stage (the opening through which the measurement light hits is approximately 1 cm in diameter) so that the letter "B" would fit inside. Then, using a 6 mm diameter sight glass, * The values ​​were measured.

[0118] <5. Film evaluation results> The angle of repose of each pellet is shown after its name. The thickness ratio of the three layers in Example 2, i.e., the skin layer / core layer / skin layer, is 15 / 70 / 15.

[0119] Regarding the pellets containing the laser marking agent (i.e., pellets B, J, L, M, E, and K), when pellet B with a repose angle of 42 degrees, pellet J with a repose angle of 32 degrees, pellet E with a repose angle of 41 degrees, and pellet K with a repose angle of 36 degrees were used, the laser marking L was significantly shorter than when pellet L with a repose angle of 55 degrees and pellet M with a repose angle of 23 degrees were used. * The variation in values ​​was small. The range of variation in the amount of laser marking agent was also small.

[0120] INDUSTRIAL APPLICABILITY The present invention can provide pellets, molded articles (for example, films and containers), and methods for producing molded articles, and is therefore industrially applicable.

Claims

1. A pellet comprising a polyolefin and a laser marking agent, the pellet having an angle of repose of 25 degrees or more and 45 degrees or less.

2. The pellet according to claim 1, wherein the content of the laser marking agent is 1% by mass or more and 50% by mass or less.

3. The pellet according to claim 1, wherein the weight of each pellet is 8 mg or more and 20 mg or less.

4. The pellets according to claim 1, used to manufacture a container.

5. A method for producing a molded product, comprising: at least a step of mixing the pellet according to any one of claims 1 to 4 and a second pellet; a step of feeding the mixed pellets prepared in the step of mixing at least the pellet and the second pellet from a hopper to an extruder; and a step of melting and extruding the mixed pellets in the extruder.

6. A method for producing a molded article according to claim 5, further comprising the step of blow molding a parison containing the layer extruded by said extruder.

7. The method for producing a molded product according to claim 5, wherein in the step of melting and extruding the mixed pellets in the extruder, a film-like melt is extruded.

8. The method for producing a molded product according to claim 5, wherein the difference between the angle of repose of the pellet and the angle of repose of the second pellet is 10 degrees or less in absolute value.

9. A film comprising a polyolefin and a laser marking agent, wherein the content of a major metal element in the laser marking agent varies by 0.10 mass% or less in the longitudinal direction of the film, and the variation is the absolute value of the difference between the average value of the content of the major metal element measured at 50 m intervals in the longitudinal direction of the film and the value furthest from the average value.

Citation Information

Patent Citations

  • Laminated material and packaging bag using it

    JP2004216740A

  • Crystal nucleator for polyolefin resins, method for producing crystal nucleator for polyolefin resins, and method for improving fluidity of crystal nucleator for polyolefin resins

    WO2018052010A1

  • Laser-printable film and packaging in which same is used

    WO2021125135A1

  • Resin raw material composition for molding use, resin raw material composition for microporous membranes, and methods respective for producing those products

    WO2022138963A1