Photosensitive composition, method for producing photosensitive composition, transfer film, laminate, and method for producing laminate
The photosensitive composition using a compound represented by formula (1) and specific dispersants addresses the challenges of light absorption and light resistance in forming high aspect ratio black patterns, achieving stable and resistant black patterns in display manufacturing.
Patent Information
- Application Number
- PCT/JP2024/010124
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-07-05
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-03
AI Technical Summary
Current methods for forming high aspect ratio black patterns in display manufacturing, such as micro LEDs, face challenges with carbon black absorption of light, leading to poor pattern shape and light-shielding properties, and leuco dye compounds exhibit poor light resistance.
A photosensitive composition containing a compound represented by formula (1) as a coloring material precursor, a dispersant with an amine value of 70 mgKOH/g or less, and additional components like an alkali-soluble resin, polymerizable monomer, and photopolymerization initiator, which suppresses light absorption and ensures excellent light resistance.
The solution enables the formation of high aspect ratio black patterns with excellent light resistance and stability, preventing unintended color development and maintaining shape integrity during exposure.
Smart Images

Figure JP2024010124_03102024_PF_FP_ABST
Abstract
Description
Photosensitive composition, method for producing photosensitive composition, transfer film, laminate, and method for producing laminate
[0001] The present disclosure relates to a photosensitive composition, a method for producing a photosensitive composition, a transfer film, a laminate, and a method for producing a laminate.
[0002] In recent years, there has been a demand for high-aspect-ratio black partition walls (so-called black matrices) in new display manufacturing methods such as micro LEDs (Light Emission Diodes). Various reports have been made on black matrices. For example, Japanese Patent Application Laid-Open No. 2022-63445 discloses a technique for forming a black matrix using a photosensitive coloring composition containing carbon black as a coloring material.
[0003] However, when carbon black is used as a colorant to form, for example, a negative-pattern black matrix, the carbon black absorbs the light (e.g., ultraviolet light) it is exposed to. This causes the incident light to gradually attenuate in the thickness direction of the composition layer used to form the pattern, and due to insufficient polymerization and curing, particularly at the bottom of the composition layer, it is difficult to obtain a pattern with a good shape after development. Therefore, a technology is needed that can suppress absorption of incident light during pattern exposure, allow the incident light to sufficiently transmit to the bottom, and ultimately form a black pattern with a good shape and excellent light-blocking properties. One such technology is, for example, a technology that uses a leuco dye compound (so-called leuco dye), which is a colorant precursor. However, black patterns formed using leuco dye compounds tend to have poor light resistance.
[0004] The present disclosure has been made in view of the above circumstances. One embodiment of the present disclosure aims to provide a photosensitive composition and a method for manufacturing the photosensitive composition that can form a black pattern having a high aspect ratio and excellent light resistance. Another embodiment of the present disclosure aims to provide a transfer film, a laminate, and a method for manufacturing the laminate that use the photosensitive composition.
[0005] Specific means for solving the above problems include the following embodiments: <1> A photosensitive composition comprising: a compound represented by the following formula (1) which is a colorant precursor; and a dispersant having an amine value of 70 mgKOH / g or less.
[0006]
[0007] In formula (1), X 1 , X 2 , X 3 , X 4 , Y 1 and Y 2 each independently represents an oxygen atom, a sulfur atom, or N-L 1 Represents L 1 represents a hydrogen atom, an alkyl group, an acyl group, an alkoxycarbonyl group, or an aminocarbonyl group. 1 , R 2 , R 3 and R 4 are each independently a hydrogen atom, -OL 2 , -OCO-L 3 , -SL 2 Or -OSO-L 3 Represents L 2 represents a hydrogen atom or an alkyl group, L 3 represents an alkyl group or an amino group. 1 and R 2 At least one of represents a hydrogen atom, and R 3 and R 4 At least one of A, B and C represents a hydrogen atom. A, B and C each independently represent an aromatic ring.
[0008] <2> The photosensitive composition according to <1>, wherein the dispersant has an acid value of 15 mgKOH / g or more. <3> The photosensitive composition according to <1> or <2>, further comprising an alkali-soluble resin, a polymerizable monomer, and a photopolymerization initiator.
[0009] <4> A method for producing a photosensitive composition, the method comprising: preparing a dispersion containing a compound represented by the following formula (1) as a colorant precursor, a dispersant having an amine value of 70 mgKOH / g or less, and a solvent; and mixing the dispersion with an alkali-soluble resin, a polymerizable monomer, and a photopolymerization initiator.
[0010]
[0011] In formula (1), X 1 , X 2 , X 3 , X 4 , Y 1 and Y 2 each independently represents an oxygen atom, a sulfur atom, or N-L 1 Represents L 1 represents a hydrogen atom, an alkyl group, an acyl group, an alkoxycarbonyl group, or an aminocarbonyl group. 1 , R 2 , R 3 and R 4 are each independently a hydrogen atom, -OL 2 , -OCO-L 3 , -SL 2 Or -OSO-L 3 Represents L 2 represents a hydrogen atom or an alkyl group, L 3 represents an alkyl group or an amino group. 1 and R 2 At least one of represents a hydrogen atom, and R 3 and R 4 At least one of A, B and C represents a hydrogen atom. A, B and C each independently represent an aromatic ring.
[0012] <5> A transfer film comprising: a temporary support; and a photosensitive composition layer containing the photosensitive composition according to any one of <1> to <3>.
[0013] <6> A method for producing a laminate having a black pattern, the method comprising: a step of forming a photosensitive composition layer containing the photosensitive composition according to any one of <1> to <3> on a substrate; a step of patternwise exposing the photosensitive composition layer; and a step of developing the photosensitive composition layer, in this order; and the method further comprising, after the step of patternwise exposing, a step of causing the compound represented by formula (1) to develop a black color.
[0014] <7> A laminate having a black pattern, the laminate being produced by the production method according to <6>. <8> The laminate according to <7>, in which the black pattern has an aspect ratio, which is the ratio of the film thickness to the line width of the bottom, of 1 or more. <9> The laminate according to <7> or <8>, in which the black pattern satisfies the relationship 0.15≦X / Y, where X is the average absorbance at a wavelength of 400 nm to 600 nm and Y μm is the film thickness.
[0015] According to one embodiment of the present disclosure, there are provided a photosensitive composition and a method for producing the photosensitive composition, which are capable of forming a black pattern having a high aspect ratio and excellent light resistance. According to another embodiment of the present disclosure, there are provided a transfer film, a laminate, and a method for producing the laminate, which use the photosensitive composition.
[0016] The present disclosure will be described in detail below. The following description of the requirements may be based on typical embodiments of the present disclosure, but the present disclosure is not limited to such embodiments and can be implemented by making appropriate modifications within the scope of the purpose of the present disclosure.
[0017] In the present disclosure, a numerical range indicated using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits, respectively. In the numerical ranges described in stages in the present disclosure, the upper or lower limit described in a certain numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Furthermore, in the numerical ranges described in the present disclosure, the upper or lower limit described in a certain numerical range may be replaced with a value shown in the examples.
[0018] In this disclosure, when referring to the amount of each component in a composition, if there are multiple substances corresponding to each component in the composition, it means the total amount of the multiple components present in the composition unless otherwise specified.
[0019] In the present disclosure, a combination of two or more preferred aspects is a more preferred aspect.
[0020] In the present disclosure, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.
[0021] In the present disclosure, "transparent" means that the average transmittance of visible light having a wavelength of 400 nm to 700 nm is 80% or more, and preferably 90% or more. In the present disclosure, "transmittance" is a value measured using a spectrophotometer. As the spectrophotometer, for example, a spectrophotometer (model number: U-3310) manufactured by Hitachi, Ltd. can be used. However, the spectrophotometer is not limited to this.
[0022] In the present disclosure, the molecular weight of a compound having a molecular weight distribution is the weight average molecular weight (Mw; the same applies hereinafter) unless otherwise specified.
[0023] In the present disclosure, unless otherwise specified, the weight average molecular weight (Mw) and number average molecular weight (Mn) are values measured by gel permeation chromatography (GPC). The GPC measurement is performed using a TSKgel® GMHxL, TSKgel® G4000HxL, or TSKgel® G2000HxL (all trade names manufactured by Tosoh Corporation) column, tetrahydrofuran (THF) as an eluent, a differential refractometer as a detector, and polystyrene as a standard substance. The values are polystyrene-equivalent values measured by a GPC analyzer.
[0024] In the present disclosure, the ratio of the constituent units of a polymer compound is a mass ratio unless otherwise specified.
[0025] In the present disclosure, "(meth)acrylic" is a term that encompasses both "acrylic" and "methacrylic," "(meth)acrylate" is a term that encompasses both "acrylate" and "methacrylate," and "(meth)acryloyloxy" is a term that encompasses both "acryloyloxy" and "methacryloyloxy."
[0026] In the present disclosure, "alkali-soluble" means that the solubility in 100 g of a 1% by mass aqueous solution of sodium carbonate at a liquid temperature of 22°C is 0.1 g or more.
[0027] In the present disclosure, "water-soluble" means that the solubility in 100 g of water having a pH of 7.0 and a liquid temperature of 22°C is 0.1 g or more. For example, "water-soluble resin" means a resin that satisfies the above solubility conditions.
[0028] In the present disclosure, the "solid content" of a composition refers to the components that form a composition layer formed using the composition, and in the case where the composition contains a solvent, refers to all components excluding the solvent. Furthermore, liquid components other than the solvent are also considered to be solids as long as they form a composition layer. In the present disclosure, the "solvent" refers to water and organic solvents.
[0029] In this disclosure, "n-" means normal, "s-" means secondary, and "t-" means tertiary.
[0030] In this disclosure, "light" refers to, for example, ultraviolet light, visible light, and infrared light. In this disclosure, "ultraviolet light" refers to light in a wavelength range of 200 nm or more and less than 400 nm, "visible light" refers to light in a wavelength range of 400 nm or more and less than 780 nm, and "infrared light" refers to light in a wavelength range of 780 nm or more and less than 1000 nm.
[0031] In the description of groups (atomic groups) in the present disclosure, descriptions that do not specify whether they are substituted or unsubstituted include those that have a substituent as well as those that do not have a substituent. For example, the term "alkyl group" includes not only alkyl groups that do not have a substituent (also referred to as "unsubstituted alkyl groups"), but also alkyl groups that have a substituent (also referred to as "substituted alkyl groups").
[0032] The "substituent" in the present disclosure is not particularly limited, and examples thereof include a halogen group, a hydroxy group, an alkyl group, a cycloalkyl group, an alkenyl group, a cycloalkenyl group, an alkynyl group, an aryl group, a heterocyclic group, an alkoxy group, an aryloxy group, a heterocyclic oxy group, a sulfo group, an acyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, a carboxy group, a carbamoyl group, an acyloxy group, a carbamoyloxy group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an alkoxyalkyleneoxy group, a cyano group, a nitro group, an amino group (including an anilino group), an acyl group, an aryloxy group, an aryloxycarbonyloxy group, an alkoxyalkyleneoxy group, a cyano group, a nitro group, an amino group (including an anilino group), an acyl group, an aryloxy group, an aryloxy group, an alkoxyalkyleneoxy group, a cyano group, a nitro group, an amino group (including an anilino group), an acyl group, an aryloxy group, an aryloxy group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an alkoxyalkyleneoxy group, a cyano group, a nitro group, an amino group (including an anilino group), an acyl group, an aryloxy ...aryloxy group, an alkoxyalkyleneoxy group, a cyano group, a nitro group, an acyl group, an aryloxy group, an aryloxy group, an aryloxy group, an aryloxy group, an alkoxyalkyleneoxy group, a cyano group, a The substituent can be arbitrarily selected from the group consisting of an amino group, an aminocarbonylamino group, an alkoxycarbonylamino group, an aryloxycarbonylamino group, a sulfamoylamino group, an alkylsulfonylamino group, an arylsulfonylamino group, a mercapto group, an alkylthio group, an arylthio group, a heterocyclic thio group, a sulfamoyl group, an alkylsulfinyl group, an arylsulfinyl group, an alkylsulfonyl group, an arylsulfonyl group, an arylazo group, a heterocyclic azo group, an imido group, a phosphino group, a phosphinyl group, a phosphinyloxy group, and a phosphinylamino group.
[0033] More specifically, examples of the substituent in the present disclosure include halogen groups (e.g., fluoro, chloro, bromo, and iodo groups), alkyl groups (linear, branched, or cyclic alkyl groups having 1 to 10, preferably 1 to 6, carbon atoms; e.g., methyl, ethyl, n-propyl, isopropyl, t-butyl, n-octyl, 2-chloroethyl, 2-cyanoethyl, and 2-ethylhexyl groups), cycloalkyl groups (preferably, cyclopropyl, and cyclohexyl), and alkyl groups (preferably, cyclopropyl, and cyclohexyl). a cycloalkenyl group (preferably a cyclopenten-1-yl group), an alkenyl group (a straight-chain, branched or cyclic alkenyl group having 2 to 10, preferably 2 to 6 carbon atoms; for example, a vinyl group, an allyl group, and a prenyl group), a cycloalkenyl group (preferably a cyclopenten-1-yl group), an alkynyl group (an alkynyl group having 2 to 10, preferably 2 to 6 carbon atoms; for example, an ethynyl group and a propargyl group), an aryl group (an aryl group having 6 to 12, preferably 6 to 8 carbon atoms; for example, a phenyl group ... a phenyl group, a p-tolyl group, a naphthyl group, a 3-chlorophenyl group, and a 2-aminophenyl group), a heterocyclic group (a monovalent group having 1 to 12, preferably 2 to 6, carbon atoms obtained by removing one hydrogen atom from a 5- or 6-membered aromatic or non-aromatic heterocyclic compound; for example, a 1-pyrazolyl group, a 1-imidazolyl group, a 2-furyl group, a 2-thienyl group, a 4-pyrimidinyl group, and a 2-benzothiazolyl group), a cyano group, a hydroxy group, a nitro group, an alkoxy group, groups (linear, branched, or cyclic alkoxy groups having 1 to 10, preferably 1 to 6, carbon atoms; for example, methoxy, ethoxy, isopropoxy, t-butoxy, cyclopentyloxy, 2-buten-1-yloxy, and 2-methoxyethoxy groups), aryloxy groups (aryloxy groups having 6 to 12, preferably 6 to 8, carbon atoms; for example, phenoxy, 2-methylphenoxy, 4-t-butylphenoxy, and 3-nitrophenoxy groups),
[0034] heterocyclic oxy groups (heterocyclic oxy groups having 1 to 12, preferably 2 to 6, carbon atoms; for example, 1-phenyltetrazole-5-oxy-2-tetrahydropyranyloxy group), acyloxy groups (acyloxy groups having 1 to 12, preferably 1 to 8, carbon atoms; for example, formyloxy group, acetyloxy group, pivaloyloxy group, benzoyloxy group, and p-methoxyphenylcarbonyloxy group), carbamoyloxy group (a carbamoyloxy group having 1 to 10, preferably 1 to 6, carbon atoms; for example, an N,N-dimethylcarbamoyloxy group, an N,N-diethylcarbamoyloxy group, a morpholinocarbonyloxy group, and an N,N-octylcarbamoyloxy group), an alkoxycarbonyloxy group (an alkoxycarbonyloxy group having 2 to 10, preferably 2 to 6, carbon atoms; for example, a methoxycarbonyloxy group, an ethoxycarbonyloxy group, a t-butoxycarbonyloxy group, and an n-octyloxycarbonyloxy group), an aryloxycarbonyloxy group (an aryloxycarbonyloxy group having 7 to 12, preferably 7 to 10, carbon atoms; for example, a phenoxycarbonyloxy group and a p-methoxyphenoxycarbonyl oxy group), amino group (amino group; alkylamino group having 1 to 10, preferably 1 to 6 carbon atoms; an anilino group having 6 to 12, preferably 6 to 8 carbon atoms; or heterocyclic amino group having 1 to 12, preferably 2 to 6 carbon atoms; for example, amino group, methylamino group, dimethylamino group, anilino group, N-methyl-anilino group, diphenylamino group, imidazol-2-ylamino group, and pyrazol-3-ylamino group), acylamino group (alkylcarbonylamino group having 1 to 10, preferably 1 to 6 carbon atoms; arylcarbonylamino group having 6 to 12, preferably 6 to 8 carbon atoms; or heterocyclic carbonylamino group having 2 to 12, preferably 2 to 6 carbon atoms;For example, a formylamino group, an acetylamino group, a pivaloylamino group, a benzoylamino group, a pyridine-4-carbonylamino group, and a thiophene-2-carbonylamino group are included), an aminocarbonylamino group (an aminocarbonylamino group having 1 to 12, preferably 1 to 6, carbon atoms; for example, a carbamoylamino group, an N,N-dimethylaminocarbonylamino group, an N,N-diethylaminocarbonylamino group, and a morpholin-4-ylcarbonylamino group), an alkoxycarbonylamino group (an alkoxycarbonylamino group having 2 to 10, preferably 2 to 6 carbon atoms; for example, a methoxycarbonylamino group, an ethoxycarbonylamino group, and a t-butoxycarbonylamino group);
[0035] an aryloxycarbonylamino group (an aryloxycarbonylamino group having 7 to 12, preferably 7 to 9, carbon atoms; for example, a phenoxycarbonylamino group, a p-chlorophenoxycarbonylamino group, and a 4-methoxyphenoxycarbonylamino group); a sulfamoylamino group (a sulfamoylamino group having 0 to 10, preferably 0 to 6, carbon atoms; for example, a sulfamoylamino group, an N,N-dimethylaminosulfonylamino group, and an N-(2-hydroxyethyl)sulfamoylamino group); amino group), alkylsulfonylamino group (an alkylsulfonylamino group having 1 to 10, preferably 1 to 6, carbon atoms; for example, a methylsulfonylamino group and a butylsulfonylamino group), arylsulfonylamino group (an arylsulfonylamino group having 6 to 12, preferably 6 to 8, carbon atoms; for example, a phenylsulfonylamino group, a 2,3,5-trichlorophenylsulfonylamino group, and a p-methylphenylsulfonylamino group), a mercapto group, an alkylthio group (1 to 10, alkylthio groups (preferably having 1 to 6 carbon atoms; for example, methylthio, ethylthio, and butylthio groups), arylthio groups (arylthio groups having 6 to 12, preferably 6 to 8 carbon atoms; for example, phenylthio, p-chlorophenylthio, and m-methoxythio groups), heterocyclic thio groups (heterocyclic thio groups having 2 to 10, preferably 1 to 6 carbon atoms; for example, 2-benzothiazolylthio and 1-phenyltetrazol-5-ylthio groups), sulfamoyl groups (0 to 10, preferably Preferably, a sulfamoyl group having 0 to 6 carbon atoms; for example, a sulfamoyl group, an N-ethylsulfamoyl group, an N,N-dimethylsulfamoyl group, an N-acetylsulfamoyl group, and an N-benzoylsulfamoyl group), an alkylsulfinyl group (an alkylsulfinyl group having 1 to 10, preferably 1 to 6, carbon atoms; for example, a methylsulfinyl group and an ethylsulfinyl group), an arylsulfinyl group (an arylsulfinyl group having 6 to 12, preferably 6 to 8, carbon atoms;For example, a phenylsulfinyl group and a p-methylphenylsulfinyl group), an alkylsulfonyl group (an alkylsulfonyl group having 1 to 10, preferably 1 to 6 carbon atoms; for example, a methylsulfonyl group and an ethylsulfonyl group), an arylsulfonyl group (an arylsulfonyl group having 6 to 12, preferably 6 to 8 carbon atoms; for example, a phenylsulfonyl group and a p-chlorophenylsulfonyl group), a sulfo group, an acyl group (a formyl group; an alkylcarbonyl group having 2 to 10, preferably 2 to 6 carbon atoms; or an arylcarbonyl group having 7 to 12, preferably 7 to 9 carbon atoms; for example, an acetyl group, a pivaloyl group, a 2-chloroacetyl group, a benzoyl group, and a 2,4-dichlorobenzoyl group);
[0036] Alkoxycarbonyl groups (alkoxycarbonyl groups having 2 to 10, preferably 2 to 6, carbon atoms; for example, methoxycarbonyl, ethoxycarbonyl, t-butoxycarbonyl, and isobutyloxycarbonyl groups), aryloxycarbonyl groups (aryloxycarbonyl groups having 7 to 12, preferably 7 to 9, carbon atoms; for example, phenoxycarbonyl-2-chlorophenoxycarbonyl, 3-nitrophenoxycarbonyl, and 4-t-butylphen ... a carbamoyl group (a carbamoyl group having 1 to 10, preferably 1 to 6, carbon atoms; for example, a carbamoyl group, an N-methylcarbamoyl group, an N,N-dimethylcarbamoyl group, an N-(2-hydroxyethyl)carbamoyl group, and an N-(methylsulfonyl)carbamoyl group), an arylazo group (an arylazo group having 6 to 12, preferably 6 to 8, carbon atoms; for example, a phenylazo group and a p-chlorophenylazo group), a heterocyclic azo group (a heterocyclic azo group having 1 to 10, preferably 1 to 6, carbon atoms), for example, a pyrazol-3-ylazo group, a thiazol-2-ylazo group, and a 5-methylthio-1,3,4-thiadiazol-2-ylazo group), an imido group (an imido group having 2 to 10, preferably 4 to 8 carbon atoms; for example, a succinimido group and a phthalimido group), a phosphino group (a phosphino group having 2 to 12, preferably 2 to 6 carbon atoms; for example, a dimethylphosphino group, a diphenylphosphino group, and a methylphenoxyphosphino group), a phosphinyl group (a phosphinyl ... carbon atoms, preferably phosphinyl groups having 2 to 12, preferably 2 to 6, carbon atoms; for example, a phosphinyl group and a diethoxyphosphinyl group), phosphinyloxy groups (phosphinyloxy groups having 2 to 12, preferably 2 to 6, carbon atoms; for example, a diphenoxyphosphinyloxy group and a dibutoxyphosphinyloxy group), and phosphinylamino groups (phosphinylamino groups having 2 to 12, preferably 2 to 6, carbon atoms; for example, a dimethoxyphosphinylamino group and a dimethylaminophosphinylamino group).
[0037] When these groups are groups that can be further substituted, these groups can further contain substituents. When these groups are substituted with two or more substituents, these substituents may be the same or different.
[0038] [Photosensitive Composition] The photosensitive composition of the present disclosure includes a compound represented by formula (1) which is a colorant precursor, and a dispersant having an amine value of 70 mgKOH / g or less. Because the photosensitive composition of the present disclosure has the above-described configuration, it can form a black pattern having a high aspect ratio and excellent light resistance.
[0039] Carbon black has traditionally been used as a colorant for forming black matrices. However, when carbon black is used as a colorant to form, for example, a negative-pattern black matrix, the carbon black absorbs the light (e.g., ultraviolet light) it is exposed to. This causes the incident light to gradually attenuate in the thickness direction of the composition layer used to form the pattern, and insufficient polymerization and curing, particularly at the bottom of the composition layer, makes it difficult to obtain a well-shaped pattern after development. In response to this problem, the present inventors have considered using a compound that develops black upon thermal stimulation. With such a compound, the timing of color development can be controlled by the timing of thermal stimulation. For example, by performing patterned exposure before color development and then subjecting the compound to black color development upon thermal stimulation after pattern exposure, it is expected that a well-shaped black pattern can be formed. The present inventors have developed a compound represented by formula (1) as a compound that develops black upon thermal stimulation. Because the compound represented by formula (1) has low solubility in solvents, it is dispersed in a photosensitive composition. However, it has been found that photosensitive compositions containing the compound represented by formula (1) in a dispersed state may gradually blacken over time. In this regard, the present inventors have conducted extensive research and found that adjusting the amine value of the dispersant used to disperse the compound represented by formula (1) to a specific value or less is effective in suppressing unintended color development of the compound represented by formula (1) before thermal stimulation. The photosensitive composition of the present disclosure contains the compound represented by formula (1) in combination with a dispersant having an amine value of a specific value or less, thereby suppressing unintended color development of the compound represented by formula (1) before thermal stimulation. Therefore, the photosensitive composition of the present disclosure can suppress absorption of incident light during patterned exposure and allow the incident light to transmit, thereby forming a black pattern with a good shape, in other words, a high aspect ratio, after development.
[0040] Leuco dye compounds have been known as colorant precursors that develop a black color. However, black patterns formed using leuco dye compounds tend to have poor lightfastness. In contrast, the photosensitive composition of the present disclosure contains a compound represented by formula (1), which allows the formation of a black pattern with excellent lightfastness. The reason for this is believed to be as follows: A leuco dye compound develops color when the lactone ring in the molecule reacts with an acid to open the ring. The above reaction in this leuco dye compound is a reversible reaction. On the other hand, the compound represented by formula (1) develops a black color upon thermal stimulation. The mechanism by which the compound represented by formula (1) develops a black color is unclear, but the inventors speculate as follows: When heated, the compound represented by formula (1) is thought to react with oxygen in the air, changing its structure to an oxidant, thereby developing a black color. In other words, it is thought that thermal stimulation acts as a trigger to change the structure of the compound represented by formula (1), and the oxidant, which is thermally oxidized from the compound represented by formula (1), exhibits a black color. Specifically, for example, the compound represented by formula (1) reacts with oxygen in the air to form a compound represented by formula (1) R 1 , R 2 , R 3 and R 4 is eliminated (e.g., dehydration, dealcoholization, etc.), and R 1 and R 2 Between 3 and R 4 It is believed that the single bond between the compound and the compound becomes a double bond, and the conjugation is extended, resulting in a change to a structure that absorbs visible light, resulting in black color development. The color development reaction of the compound represented by formula (1) is an irreversible reaction, unlike that of leuco dye compounds. For this reason, it is believed that the black pattern formed by the photosensitive composition according to the present disclosure containing the compound represented by formula (1) has excellent light resistance.
[0041] The photosensitive composition of the present disclosure can also exhibit the effect of excellent dispersion stability of the compound represented by formula (1). Furthermore, as described above, the photosensitive composition of the present disclosure can exhibit the effect of excellent color stability over time because unintended color development of the compound represented by formula (1) before thermal stimulation is suppressed.
[0042] In the present disclosure, the “compound represented by formula (1) that is a colorant precursor” is also simply referred to as the “compound represented by formula (1).” In addition, in the present disclosure, the “dispersant having an amine value of 70 mgKOH / g or less” is also referred to as the “specific dispersant.”
[0043] <Compound Represented by Formula (1)> The photosensitive composition of the present disclosure contains a compound represented by formula (1). The compound represented by formula (1) is a colorant precursor, and develops a black color upon thermal stimulation (for example, heating at 80°C to 260°C).
[0044] The compound represented by formula (1) is preferably a compound that satisfies the following requirements A, B, and C.
[0045] (Requirement A) In the absorption spectrum measured using a spectrophotometer for a solution prepared by dissolving 1.1 mg of the compound before color development in 50 mL of tetrahydrofuran (THF), the average value of the molar absorption coefficient (ε) at any consecutive 100 nm wavelengths within the wavelength range of 400 nm to 700 nm (so-called average molar absorption coefficient) is 400 L / (mol cm) or less.
[0046] The average molar absorption coefficient in requirement A is preferably 200 L / (mol·cm) or less, and more preferably 100 L / (mol·cm) or less.
[0047] The average value of the molar absorption coefficient (ε) at successive 100 nm wavelengths within the wavelength range of 400 nm to 700 nm can be determined by determining the molar absorption coefficient at each wavelength in 1 nm increments and then arithmetically averaging the molar absorption coefficients in successive 100 nm ranges (e.g., 421 nm to 520 nm, 560 nm to 659 nm, etc.). The same applies to requirement C described below.
[0048] "The average value of the molar absorption coefficient (ε) over any consecutive 100 nm wavelengths within a wavelength range of 400 nm to 700 nm is 400 L / (mol cm) or less" means that, regardless of which consecutive 100 nm wavelength range is selected within the wavelength range of 400 nm to 700 nm, the average molar absorption coefficient over that consecutive 100 nm wavelength range is 400 L / (mol cm) or less.
[0049] (Requirement B) In the absorption spectrum measured using a spectrophotometer for a solution prepared by dissolving 1.1 mg of the color-developed compound in 50 mL of tetrahydrofuran (THF), the maximum absorption wavelength is within the wavelength range of 400 nm to 700 nm.
[0050] The number of absorption maximum wavelengths within the wavelength range of 400 nm to 700 nm is preferably 2 or more. The upper limit of the number of absorption maximum wavelengths within the wavelength range of 400 nm to 700 nm is not particularly limited, and examples thereof include 10 or less, 5 or less, 3 or less, etc.
[0051] When there are two or more maximum absorption wavelengths within the wavelength range of 400 nm to 700 nm, the maximum absorption wavelengths are preferably separated by 100 nm or more, and more preferably by 200 nm or more.
[0052] The molar extinction coefficient (ε) at the wavelength where absorption is maximum among the above-mentioned maximum absorption wavelengths in the wavelength range of 400 nm to 700 nm is preferably 3000 L / (mol cm) or more, more preferably 4000 L / (mol cm) or more, and even more preferably 5000 L / (mol cm) or more. Furthermore, the molar extinction coefficient (ε) at the wavelength where absorption is maximum among the above-mentioned maximum absorption wavelengths in the wavelength range of 400 nm to 700 nm is preferably 100,000 L / (mol cm) or less, more preferably 40,000 L / (mol cm) or less, and even more preferably 20,000 L / (mol cm) or less.
[0053] (Requirement C) In the absorption spectrum measured using a spectrophotometer for a solution prepared by dissolving 1.1 mg of the color-developed compound in 50 mL of tetrahydrofuran (THF), the average value of the molar absorption coefficient (ε) at any consecutive 100 nm wavelengths within the wavelength range of 400 nm to 700 nm (i.e., the average molar absorption coefficient) is 2000 L / (mol cm) or more.
[0054] The average molar absorption coefficient in requirement C is preferably 3000 L / (mol·cm) or more, and more preferably 4000 L / (mol·cm) or more.
[0055] "The average value of the molar absorption coefficient (ε) over any consecutive 100 nm wavelengths within a wavelength range of 400 nm to 700 nm is 2000 L / (mol cm) or more" means that, regardless of which consecutive 100 nm wavelength range is selected within the wavelength range of 400 nm to 700 nm, the average molar absorption coefficient over that consecutive 100 nm wavelength range is 2000 L / (mol cm) or more.
[0056] The compound represented by formula (1) will be described in detail below.
[0057]
[0058] In formula (1), X 1 , X 2 , X 3 , X 4 , Y 1 and Y 2 each independently represents an oxygen atom, a sulfur atom, or N-L 1 Represents.
[0059] X 1 , X 2 , X 3 and X 4 is preferably an oxygen atom.
[0060] In formula (1), there are two Y 1 may be the same or different, but are preferably the same. 1 is preferably an oxygen atom.
[0061] In formula (1), there are two Y 2 may be the same or different, but are preferably the same. 2 is N-L 1 It is preferable that L 1 represents a hydrogen atom, an alkyl group, an acyl group, an alkoxycarbonyl group, or an aminocarbonyl group, preferably a hydrogen atom, an alkyl group, an acyl group, or an alkoxycarbonyl group, and more preferably an alkyl group, an acyl group, or an alkoxycarbonyl group.
[0062] L 1The alkyl group represented by the formula (I) may or may not have a substituent. 1 The alkyl group represented by the formula (I) may be a linear alkyl group, a branched alkyl group, or an alkyl group having a cyclic structure. 1 The alkyl group represented by the formula (I) is preferably an alkyl group having 1 to 30 carbon atoms, and more preferably an alkyl group having 1 to 12 carbon atoms. 1 The alkyl group represented by the formula (I) is preferably, for example, an s-butyl group, an n-hexyl group, a 2-ethoxyethyl group, a methoxycarbonylmethyl group, an isopropyl group, an n-pentyl group or a 2-ethylhexyl group.
[0063] L 1 The acyl group represented by the formula (I) is preferably an acyl group having 2 to 30 carbon atoms, and more preferably an acyl group having 2 to 15 carbon atoms. 1 The acyl group represented by the formula (I) is preferably, for example, an acetyl group, a 2-ethylhexanoyl group, a 3,3,5-trimethylhexanoyl group, a propionyl group, a butyryl group, an isobutyryl group or a pivaloyl group.
[0064] L 1 The alkoxycarbonyl group represented by the formula (I) is preferably an alkoxycarbonyl group having 1 to 30 carbon atoms in the alkoxy moiety. 1 The alkoxycarbonyl group represented by the formula (I) is preferably, for example, a methoxycarbonyl group, an ethoxycarbonyl group, a butoxycarbonyl group, a t-butoxycarbonyl group, a 9-fluorenylmethyloxycarbonyl group, a benzyloxycarbonyl group or a 2,2,2-trichloroethyloxycarbonyl group.
[0065] R 1 , R 2 , R 3 and R 4 are each independently a hydrogen atom, -OL 2 , -OCO-L 3 , -SL 2 Or -OSO-L 3 Represents L 2 represents a hydrogen atom or an alkyl group, L 3represents an alkyl group or an amino group. 1 and R 2 At least one of represents a hydrogen atom, and R 3 and R 4 At least one of these represents a hydrogen atom.
[0066] R 1 and R 2 When one of the groups is a hydrogen atom, the other group is a hydrogen atom or a hydroxy group (i.e., L 2 is a hydrogen atom 2 ), and more preferably a hydrogen atom. 3 and R 4 When one of the groups is a hydrogen atom, the other group is a hydrogen atom or a hydroxy group (i.e., L 2 is a hydrogen atom 2 ), and more preferably a hydrogen atom.
[0067] L 2 is preferably a hydrogen atom. 2 The alkyl group represented by the formula (I) may or may not have a substituent. 2 The alkyl group represented by the formula (I) may be a linear alkyl group, a branched alkyl group, or an alkyl group having a cyclic structure. 2 The alkyl group represented by the formula (I) is preferably an alkyl group having 1 to 30 carbon atoms, and more preferably an alkyl group having 1 to 12 carbon atoms. 2 The alkyl group represented by the formula (I) is preferably, for example, a methyl group, an ethyl group, a propyl group or a 2-ethylhexyl group.
[0068] L 3 The alkyl group represented by the formula (I) may or may not have a substituent. 3 The alkyl group represented by the formula (I) may be a linear alkyl group, a branched alkyl group, or an alkyl group having a cyclic structure. 3 The alkyl group represented by the formula (I) is preferably an alkyl group having 1 to 30 carbon atoms, and more preferably an alkyl group having 1 to 12 carbon atoms.3 The alkyl group represented by the formula (I) is preferably, for example, a methyl group, an ethyl group, a propyl group or a 2-ethylhexyl group.
[0069] A, B, and C each independently represent an aromatic ring.
[0070] The aromatic ring represented by A and the aromatic ring represented by B may be the same or different. The aromatic rings represented by A and B may or may not have a substituent. The aromatic rings represented by A and B may be, for example, an aromatic hydrocarbon ring, an aromatic heterocycle, or a condensed ring thereof.
[0071] When the aromatic rings represented by A and B are aromatic hydrocarbon rings, the aromatic hydrocarbon rings represented by A and B are preferably 5- or 6-membered rings, and more preferably 6-membered rings. When the aromatic rings represented by A and B are aromatic hydrocarbon rings, the aromatic hydrocarbon rings represented by A and B are preferably aromatic hydrocarbon rings having 6 to 30 carbon atoms, more preferably aromatic hydrocarbon rings having 6 to 20 carbon atoms, and even more preferably aromatic hydrocarbon rings having 6 to 10 carbon atoms. When the aromatic rings represented by A and B are aromatic hydrocarbon rings, the aromatic hydrocarbon ring represented by A is preferably, for example, a benzene ring, a naphthalene ring, or an anthracene ring, and more preferably a benzene ring.
[0072] When the aromatic rings represented by A and B are aromatic heterocycles, the aromatic heterocycles represented by A and B are preferably 5- or 6-membered rings, more preferably 5-membered rings. When the aromatic rings represented by A and B are aromatic heterocycles, the aromatic heterocycles represented by A and B are preferably aromatic heterocycles containing one or more heteroatoms selected from the group consisting of oxygen atoms, sulfur atoms, and nitrogen atoms in the ring. The number of heteroatoms in the aromatic heterocycle is preferably 1 or 2, more preferably 1. When the aromatic rings represented by A and B are aromatic heterocycles, the aromatic heterocycles represented by A and B are preferably, for example, a thiophene ring, a furan ring, a pyrrole ring, an imidazole ring, a triazole ring, or a pyridine ring, and more preferably a thiophene ring.
[0073] The aromatic ring represented by C may or may not have a substituent. Examples of the aromatic ring represented by C include a benzene ring and an aromatic heterocycle. Examples of the heterocycle include a pyridine ring and a pyrazine ring. The aromatic ring represented by C is preferably a benzene ring.
[0074] In formula (1), X 1 , X 2 , X 3 , X 4 , R 1 , R 2 , R 3 and R 4 For example, the following aspect A is preferred, and aspect B is more preferred. Aspect A: X 1 , X 2 , X 3 and X 4 is an oxygen atom, and R 1 and R 2 is a hydrogen atom on one side and a hydroxy group on the other side, and R 3 and R 4 In the embodiment B, one of X is a hydrogen atom and the other is a hydroxy group. 1 , X 2 , X 3 and X 4 is an oxygen atom, and R 1 , R 2 , R 3 and R 4 is a hydrogen atom.
[0075] A preferred embodiment of the compound represented by formula (1) is X 1 , X 2 , X 3 and X 4 is an oxygen atom, and Y 1 and Y 2 each independently represents an oxygen atom, a sulfur atom, or N-L 1 and L 1 is a hydrogen atom, an alkyl group, an acyl group, or an alkoxycarbonyl group, and R 1 or R 2 one of which is a hydrogen atom and the other is a hydroxy group, and R 3 or R 4A and B are each independently a benzene ring or a thiophene ring, and C is a benzene ring. 1 , X 2 , X 3 and X 4 is an oxygen atom, and Y 1 is an oxygen atom, and Y 2 But N-L 1 and L 1 is an alkyl group, an acyl group, or an alkoxycarbonyl group, and R 1 , R 2 , R 3 and R 4 is a hydrogen atom, A and B are benzene rings, and C is a benzene ring.
[0076] Specific examples of the compound represented by formula (1) are listed below. However, the compound represented by formula (1) is not limited to the following specific examples. Note that "Me" represents a methyl group.
[0077]
[0078]
[0079]
[0080]
[0081]
[0082]
[0083]
[0084]
[0085]
[0086] As the compound represented by formula (1), among the above specific examples, at least one selected from the group consisting of compounds (1) to (16), compounds (25) to (32), and compound (65) is preferred, at least one selected from the group consisting of compounds (1) to (16), and compound (65) is more preferred, at least one selected from the group consisting of compounds (1) to (3), compounds (5), compounds (7), and compound (8) is even more preferred, at least one selected from the group consisting of compounds (1) to (3), compounds (5), compounds (7), and compound (8) is even more preferred, and at least one selected from compounds (1) and (2) is particularly preferred.
[0087] The photosensitive composition according to the present disclosure may contain one type of compound represented by formula (1) alone, or may contain two or more types.
[0088] The content of the compound represented by formula (1) in the photosensitive composition according to the present disclosure is not particularly limited, but from the viewpoint of achieving better effects of the present disclosure, the content is preferably 1% by mass to 20% by mass, more preferably 2% by mass to 15% by mass, and even more preferably 3% by mass to 10% by mass, relative to the total solid content of the photosensitive composition.
[0089] The method for producing the compound represented by formula (1) is not particularly limited. The compound represented by formula (1) can be produced by referring to known methods. For example, the compound represented by formula (1) can be produced by synthesizing an isatin derivative using isatin as a starting material with reference to known literature, then reacting the synthesized isatin derivative with 3,7-Dihydrobenzo[1,2-b:4,5-b']difuran-2,6-dione in an organic solvent in the presence of an acid catalyst, and reducing the compound obtained by the reaction. Methods for synthesizing isatin derivatives are described in, for example, J. Am. Chem. Soc. 2015, 137, 15947-15956, Journal of Medicinal Chemistry, 2008, 51, 4932-4947, Chemistry-A European Journal, 2021, 27, 4302-4306, and Org. Lett., 2021, 23, 2273-2278. The descriptions in these documents are incorporated herein by reference. Examples of organic solvents include ether-based organic solvents, with tetrahydrofuran (THF) and / or 1,4-dioxane being preferred, and tetrahydrofuran (THF) being more preferred. Examples of methods for reducing the compound obtained by the reaction include methods using reducing agents such as zinc powder, trifluoroacetic acid, acetic acid, and hydrochloric acid. Alternatively, the reduction may be catalytic reduction using a palladium catalyst. The reduction method is preferably reduction using zinc powder (so-called zinc reduction) or catalytic reduction using a palladium catalyst, with zinc reduction being more preferred. The reaction temperature is not particularly limited, but is preferably, for example, 20°C to 40°C, and more preferably 30°C to 40°C. The reaction time is not particularly limited, but is, for example, preferably 1 hour to 6 hours, and more preferably 1 hour to 2 hours. The compound represented by formula (1) can be suitably produced by the method described in the Examples below.
[0090] <Specific Dispersant> The photosensitive composition according to the present disclosure contains a dispersant having an amine value of 70 mgKOH / g or less (i.e., a specific dispersant).
[0091] The specific dispersant is not particularly limited as long as it has an amine value of 70 mgKOH / g or less. The specific dispersant is preferably a polymer having a basic functional group. Examples of the basic functional group include an amino group, an imino group, an amide group, and an imide group. From the viewpoint of dispersibility, the basic functional group is preferably an amino group.
[0092] The amine value of the specific dispersant is 70 mgKOH / g or less. When the amine value of the dispersant is 70 mgKOH / g or less, a black pattern with a high aspect ratio tends to be formed. Furthermore, the compound represented by formula (1) is less likely to develop an unintended color before color development due to thermal stimulation, and the photosensitive composition tends to have excellent color stability over time. From this perspective, the amine value of the specific dispersant is preferably 55 mgKOH / g or less, more preferably 40 mgKOH / g or less, and even more preferably 25 mgKOH / g or less. The lower limit of the amine value of the specific dispersant is not particularly limited, and examples include 0 mgKOH / g or more. For example, from the viewpoint of the dispersion stability of the compound represented by formula (1), the amine value of the specific dispersant is preferably more than 0 mgKOH / g, preferably 5 mgKOH / g or more, more preferably 10 mgKOH / g or more, and particularly preferably 15 mgKOH / g or more. In one embodiment, the amine value of the specific dispersant may be in the range of 0 mgKOH / g or more and 70 mgKOH / g or less, more than 0 mgKOH / g to 70 mgKOH / g or less, 5 mgKOH / g or more and 55 mgKOH / g or less, 10 mgKOH / g or more and 40 mgKOH / g or less, or 15 mgKOH / g or more and 25 mgKOH / g or less.
[0093] The amine value is the number of milligrams of potassium hydroxide equivalent to the amount of hydrochloric acid required to neutralize 1 g of sample. In this disclosure, the amine value of a dispersant is measured by potentiometric titration in accordance with JIS K 7237:1995. In addition, when the dispersant is a commercially available product and the amine value is listed in the catalog of the commercially available product, the amine value listed in the catalog is used as the reference.
[0094] The acid value of the specific dispersant is not particularly limited, but is preferably 15 mgKOH / g or more, more preferably 20 mgKOH / g or more, and even more preferably 30 mgKOH / g or more. When the acid value of the specific dispersant is 15 mgKOH / mg or more, the dispersion stability of the compound represented by formula (1) in the photosensitive composition tends to be further improved. The upper limit of the acid value of the specific dispersant is not particularly limited, and may be, for example, 200 mgKOH / mg or less. In one embodiment, the acid value of the specific dispersant may be in the range of 15 mgKOH / g or more to 200 mgKOH / mg or less, 20 mgKOH / g or more to 150 mgKOH / mg or less, or 30 mgKOH / g or more to 100 mgKOH / mg or less.
[0095] The acid value is the number of milligrams of potassium hydroxide required to neutralize 1 g of sample. In the present disclosure, the acid value of a dispersant is measured by a neutralization titration method in accordance with JIS K 0070:1992. In addition, when the dispersant is a commercially available product and the acid value is listed in the catalog of the commercially available product, the acid value listed in the catalog is used as the basis.
[0096] Commercially available products can be used as the specific dispersant. Examples of commercially available specific dispersants include "Ajisper (registered trademark) PA111" (amine value: 0 mgKOH / g, acid value: 35 mgKOH / g, manufactured by Ajinomoto Fine-Techno Co., Ltd.), "Disparlon (registered trademark) PW-36" [amine value: 0 mgKOH / g, acid value: 55 mgKOH / g, manufactured by Kusumoto Chemicals Co., Ltd.], "DISPERBYK (registered trademark)-111" [amine value: 0 mgKOH / g, acid value: 129 mgKOH / g, manufactured by BYK Japan Co., Ltd.], "DISPERBYK (registered trademark)-2001" [amine value: 29 mgKOH / g, acid value: 19 mgKOH / g, manufactured by BYK Japan Co., Ltd.], "DISPERBYK (registered trademark)-2025" [amine value: 37 mgKOH / g, acid value: 38 mgKOH / g, manufactured by BYK Japan Co., Ltd.], "DISPERBYK (registered trademark)-164" [amine value: 18 mgKOH / g, acid value: 0 mgKOH / g, manufactured by BYK Japan Co., Ltd.], and "AJISPER (registered trademark) PN411" (amine value: 0 mgKOH / g, acid value: 6 mgKOH / g, manufactured by Ajinomoto Fine-Techno Co., Ltd.).
[0097] The photosensitive composition according to the present disclosure may contain one type of specific dispersant alone, or may contain two or more types of specific dispersants.
[0098] The content of the specific dispersant in the photosensitive composition according to the present disclosure is not particularly limited, but from the viewpoint of the dispersibility of the compound represented by formula (1), the content is preferably 0.002 to 0.05 times, more preferably 0.003 to 0.03 times, and even more preferably 0.004 to 0.02 times, the amount of the compound represented by formula (1) on a mass basis.
[0099] <Other Components> The photosensitive composition according to the present disclosure may further contain an alkali-soluble resin, a polymerizable monomer, and a photopolymerization initiator in addition to the compound represented by formula (1) and the specific dispersant. The photosensitive composition according to the present disclosure may also contain additives such as a heterocyclic compound, an aliphatic thiol compound, a thermally crosslinkable compound, a surfactant, a polymerization inhibitor, a hydrogen donor compound, and a solvent. These components will be described in detail below.
[0100] <Alkali-Soluble Resin> The photosensitive composition according to the present disclosure may contain an alkali-soluble resin. Examples of alkali-soluble resins include (meth)acrylic resins, styrene resins, epoxy resins, amide resins, amide-epoxy resins, alkyd resins, phenolic resins, ester resins, urethane resins, epoxy acrylate resins obtained by reacting an epoxy resin with (meth)acrylic acid, and acid-modified epoxy acrylate resins obtained by reacting an epoxy acrylate resin with an acid anhydride.
[0101] A preferred embodiment of the alkali-soluble resin is a (meth)acrylic resin, from the viewpoint of excellent alkali developability and film formability. In the present disclosure, (meth)acrylic resin refers to a resin containing structural units derived from (meth)acrylic compounds. The content of structural units derived from (meth)acrylic compounds is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, based on the total structural units of the (meth)acrylic resin. The (meth)acrylic resin may be composed solely of structural units derived from (meth)acrylic compounds, or may also contain structural units derived from polymerizable monomers other than (meth)acrylic compounds. In other words, the upper limit of the content of structural units derived from (meth)acrylic compounds may be 100% by mass, based on the total structural units of the (meth)acrylic resin.
[0102] Examples of (meth)acrylic compounds include (meth)acrylic acid, (meth)acrylic acid esters, (meth)acrylamide, and (meth)acrylonitrile. Examples of (meth)acrylic acid esters include (meth)acrylic acid alkyl esters, (meth)acrylic acid tetrahydrofurfuryl esters, (meth)acrylic acid dimethylaminoethyl esters, (meth)acrylic acid diethylaminoethyl esters, (meth)acrylic acid glycidyl esters, (meth)acrylic acid benzyl esters, 2,2,2-trifluoroethyl (meth)acrylate, and 2,2,3,3-tetrafluoropropyl (meth)acrylate, with (meth)acrylic acid alkyl esters being preferred. Examples of (meth)acrylamides include acrylamides such as diacetone acrylamide.
[0103] The alkyl group of the (meth)acrylic acid alkyl ester may be linear or branched. Specific examples of the (meth)acrylic acid alkyl ester include (meth)acrylic acid alkyl esters having an alkyl group having 1 to 12 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, and dodecyl (meth)acrylate. The (meth)acrylic acid alkyl ester is preferably a (meth)acrylic acid alkyl ester having an alkyl group having 1 to 4 carbon atoms, and more preferably methyl (meth)acrylate or ethyl (meth)acrylate.
[0104] The (meth)acrylic resin may contain a structural unit other than the structural unit derived from the (meth)acrylic compound. The polymerizable monomer that forms the structural unit other than the structural unit derived from the (meth)acrylic compound is not particularly limited as long as it is a compound other than the (meth)acrylic compound that is copolymerizable with the (meth)acrylic compound. Examples of compounds other than the (meth)acrylic compound that are copolymerizable with the (meth)acrylic compound include styrene compounds that may have a substituent at the α-position or aromatic ring, such as styrene, vinyl toluene, and α-methyl styrene; acrylonitrile; vinyl alcohol esters such as vinyl-n-butyl ether; maleic acid, maleic anhydride, maleic acid monoesters such as monomethyl maleate, monoethyl maleate, and monoisopropyl maleate; fumaric acid, cinnamic acid, α-cyanocinnamic acid, itaconic acid, and crotonic acid. The (meth)acrylic resin may contain one or more structural units derived from these polymerizable monomers.
[0105] From the viewpoint of improving alkaline developability, the (meth)acrylic resin preferably contains a structural unit having an acid group. Examples of the acid group include a carboxy group, a sulfo group, a phosphate group, and a phosphonate group. The (meth)acrylic resin more preferably contains a structural unit having a carboxy group, and even more preferably contains a structural unit derived from the above-mentioned (meth)acrylic acid.
[0106] When the (meth)acrylic resin contains a structural unit having an acid group in the (meth)acrylic resin (preferably a structural unit derived from (meth)acrylic acid; the same applies hereinafter), the content of the structural unit having an acid group in the (meth)acrylic resin is preferably 10% by mass or more relative to the total mass of the (meth)acrylic resin, from the viewpoint of excellent developability. The upper limit of the content of the structural unit having an acid group in the (meth)acrylic resin is preferably 50% by mass or less, more preferably 40% by mass or less, relative to the total mass of the (meth)acrylic resin, from the viewpoint of excellent alkali resistance.
[0107] The (meth)acrylic resin more preferably contains structural units derived from the aforementioned (meth)acrylic acid alkyl ester. When the (meth)acrylic resin contains structural units derived from the (meth)acrylic acid alkyl ester, the content of the structural units derived from the (meth)acrylic acid alkyl ester in the (meth)acrylic resin is preferably 1% by mass to 90% by mass, more preferably 1% by mass to 50% by mass, and even more preferably 1% by mass to 30% by mass, relative to all structural units of the (meth)acrylic resin.
[0108] The (meth)acrylic resin is preferably a resin containing both structural units derived from (meth)acrylic acid and structural units derived from (meth)acrylic acid alkyl ester as structural units, and more preferably a resin formed only from structural units derived from (meth)acrylic acid and structural units derived from (meth)acrylic acid alkyl ester. The (meth)acrylic resin may also be an acrylic resin having structural units derived from methacrylic acid, structural units derived from methyl methacrylate, and structural units derived from ethyl acrylate.
[0109] From the viewpoint of achieving superior effects of the present disclosure, the (meth)acrylic resin preferably contains at least one selected from the group consisting of structural units derived from methacrylic acid and structural units derived from methacrylic acid alkyl esters, and preferably contains both structural units derived from methacrylic acid and structural units derived from methacrylic acid alkyl esters. From the viewpoint of achieving superior effects of the present disclosure, the total content of structural units derived from methacrylic acid and structural units derived from methacrylic acid alkyl esters in the (meth)acrylic resin is preferably 40% by mass or more, more preferably 60% by mass or more, relative to the total structural units of the (meth)acrylic resin. The upper limit of the total content of structural units derived from methacrylic acid and structural units derived from methacrylic acid alkyl esters in the (meth)acrylic resin may, for example, be 100% by mass or less, and preferably 80% by mass or less.
[0110] From the viewpoint of achieving even better effects of the present disclosure, the (meth)acrylic resin may contain at least one type of structural unit selected from the group consisting of structural units derived from methacrylic acid and structural units derived from a methacrylic acid alkyl ester, and at least one type of structural unit selected from the group consisting of structural units derived from acrylic acid and structural units derived from an acrylic acid alkyl ester.
[0111] The (meth)acrylic resin preferably has an ester group at its terminal, from the viewpoint of providing a photosensitive composition layer formed using the photosensitive composition with excellent developability. The terminal portion of the (meth)acrylic resin is composed of a moiety derived from the polymerization initiator used in the synthesis. The (meth)acrylic resin having an ester group at its terminal can be synthesized by using a radical polymerization initiator having an ester group.
[0112] The alkali-soluble resin is preferably a resin having an acid value of 60 mgKOH / g or more, for example, from the viewpoint of developability. Furthermore, the alkali-soluble resin is more preferably a resin having a carboxy group with an acid value of 60 mgKOH / g or more (so-called carboxy group-containing resin), and even more preferably a (meth)acrylic resin having a carboxy group with an acid value of 60 mgKOH / g or more (so-called carboxy group-containing (meth)acrylic resin), for example, from the viewpoint of easily thermally crosslinking with a crosslinking component by heating to form a strong film. When the alkali-soluble resin is a carboxy group-containing resin, the three-dimensional crosslinking density can be increased by, for example, adding a thermally crosslinkable compound such as a blocked isocyanate compound to thermally crosslink the resin. Furthermore, when the carboxy group of the carboxy group-containing resin is anhydrous and hydrophobicized, the wet heat resistance can be improved.
[0113] The carboxyl group-containing (meth)acrylic resin having an acid value of 60 mgKOH / g or more is not particularly limited as long as it satisfies the above-mentioned acid value requirement, and can be appropriately selected from known (meth)acrylic resins. Preferred examples of the carboxyl group-containing (meth)acrylic resin having an acid value of 60 mgKOH / g or more include the carboxyl group-containing (meth)acrylic resins having an acid value of 60 mgKOH / g or more among the polymers described in paragraph
[0025] of JP-A No. 2011-95716, and the carboxyl group-containing (meth)acrylic resins having an acid value of 60 mgKOH / g or more among the polymers described in paragraphs
[0033] to
[0052] of JP-A No. 2010-237589.
[0114] Another suitable embodiment of the alkali-soluble resin is a styrene-acrylic copolymer. In the present disclosure, a styrene-acrylic copolymer refers to a resin containing structural units derived from a styrene compound and structural units derived from a (meth)acrylic compound. The total content of structural units derived from a styrene compound and structural units derived from a (meth)acrylic compound in the styrene-acrylic copolymer is, for example, preferably 30% by mass or more, and more preferably 50% by mass or more, relative to all structural units of the styrene-acrylic copolymer. The content of structural units derived from a styrene compound in the styrene-acrylic copolymer is, for example, preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 5% to 80% by mass, relative to all structural units of the styrene-acrylic copolymer. The content of structural units derived from a (meth)acrylic compound in the styrene-acrylic copolymer is, for example, preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% to 95% by mass, relative to all structural units of the styrene-acrylic copolymer.
[0115] From the viewpoint of achieving superior effects of the present disclosure, the alkali-soluble resin preferably has an aromatic ring structure, and more preferably contains a structural unit having an aromatic ring structure. Examples of monomers forming structural units having an aromatic ring structure include monomers having an aralkyl group, styrene, and polymerizable styrene derivatives (e.g., methylstyrene, vinyltoluene, tert-butoxystyrene, acetoxystyrene, 4-vinylbenzoic acid, styrene dimer, and styrene trimer). Examples of monomers forming structural units having an aromatic ring structure include monomers having an aralkyl group or styrene. Examples of aralkyl groups include substituted or unsubstituted phenylalkyl groups and substituted or unsubstituted benzyl groups, with substituted or unsubstituted benzyl groups being preferred. Examples of monomers having a phenylalkyl group include phenylethyl (meth)acrylate. Examples of the monomer having a benzyl group include (meth)acrylates having a benzyl group [e.g., benzyl (meth)acrylate and chlorobenzyl (meth)acrylate] and vinyl monomers having a benzyl group [e.g., vinylbenzyl chloride and vinylbenzyl alcohol], with benzyl (meth)acrylate being preferred.
[0116] From the viewpoint of achieving better effects of the present disclosure, the alkali-soluble resin more preferably contains a structural unit represented by the following formula (S) (i.e., a structural unit derived from styrene).
[0117]
[0118] When the alkali-soluble resin contains a constituent unit having an aromatic ring structure, the content of the constituent unit having an aromatic ring structure in the alkali-soluble resin is preferably 5% by mass to 90% by mass, more preferably 10% by mass to 70% by mass, and even more preferably 20% by mass to 60% by mass, relative to all constituent units of the alkali-soluble resin, from the viewpoint of achieving better effects of the present disclosure.
[0119] From the viewpoint of achieving superior effects of the present disclosure, the content of the structural units having an aromatic ring structure in the alkali-soluble resin is preferably 5 mol % to 70 mol %, more preferably 10 mol % to 60 mol %, and even more preferably 20 mol % to 60 mol %, relative to all structural units of the alkali-soluble resin.
[0120] From the viewpoint of achieving superior effects of the present disclosure, the content of the structural unit represented by formula (S) in the alkali-soluble resin is preferably 5 mol % to 70 mol %, more preferably 10 mol % to 60 mol %, even more preferably 20 mol % to 60 mol %, and particularly preferably 20 mol % to 50 mol %, relative to all structural units of the alkali-soluble resin.
[0121] In the present disclosure, when the content of a "structural unit" is specified as a molar ratio, the "structural unit" is synonymous with a "monomer unit." In addition, in the present disclosure, the "monomer unit" may be modified after polymerization by a polymer reaction or the like. The same applies hereinafter.
[0122] From the viewpoint of achieving superior effects of the present disclosure, the alkali-soluble resin preferably contains a structural unit having an aliphatic hydrocarbon ring structure. The aliphatic hydrocarbon ring structure may be monocyclic or polycyclic. The alkali-soluble resin may contain a structural unit having a ring structure in which two or more aliphatic hydrocarbon rings are condensed.
[0123] Examples of the aliphatic hydrocarbon ring include a tricyclodecane ring, a cyclohexane ring, a cyclopentane ring, a norbornane ring, and an isoboron ring. Examples of monomers that form a structural unit having an aliphatic hydrocarbon ring structure include dicyclopentanyl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate.
[0124] From the viewpoint of achieving better effects of the present disclosure, the alkali-soluble resin more preferably contains a constitutional unit represented by the following formula (Cy), and even more preferably contains a constitutional unit represented by the above formula (S) and a constitutional unit represented by the following formula (Cy).
[0125]
[0126] In formula (Cy), R M represents a hydrogen atom or a methyl group, R Cy represents a monovalent group having an aliphatic hydrocarbon ring structure.
[0127] R in formula (Cy) M is preferably a methyl group.
[0128] R in formula (Cy) Cy is preferably a monovalent group having an aliphatic hydrocarbon ring structure having 5 to 20 carbon atoms, more preferably a monovalent group having an aliphatic hydrocarbon ring structure having 6 to 16 carbon atoms, and even more preferably a monovalent group having an aliphatic hydrocarbon ring structure having 8 to 14 carbon atoms, from the viewpoint of achieving better effects of the present disclosure.
[0129] R in formula (Cy) Cy From the viewpoint of achieving better effects of the present disclosure, the aliphatic hydrocarbon ring structure in is preferably a cyclopentane ring structure, a cyclohexane ring structure, a tetrahydrodicyclopentadiene ring structure, a norbornane ring structure, or an isoborone ring structure, more preferably a cyclohexane ring structure or a tetrahydrodicyclopentadiene ring structure, and even more preferably a tetrahydrodicyclopentadiene ring structure.
[0130] R in formula (Cy) Cy From the viewpoint of achieving better effects of the present disclosure, the aliphatic hydrocarbon ring structure in is preferably a ring structure in which two or more aliphatic hydrocarbon rings are fused, and more preferably a ring in which two to four aliphatic hydrocarbon rings are fused.
[0131] R in formula (Cy) Cy From the viewpoint of achieving better effects of the present disclosure, is preferably a group in which the oxygen atom of —C(═O)O— in formula (Cy) is directly bonded to an aliphatic hydrocarbon ring structure, i.e., an aliphatic hydrocarbon ring group, more preferably a cyclohexyl group or a dicyclopentanyl group, and even more preferably a dicyclopentanyl group.
[0132] When the alkali-soluble resin contains a structural unit having an aliphatic hydrocarbon ring structure, it may contain one type of structural unit having an aliphatic hydrocarbon ring structure alone, or may contain two or more types of structural units having an aliphatic hydrocarbon ring structure.
[0133] When the alkali-soluble resin contains a structural unit having an aliphatic hydrocarbon ring structure, the content of the structural unit having an aliphatic hydrocarbon ring structure in the alkali-soluble resin is preferably 5% by mass to 90% by mass, more preferably 10% by mass to 80% by mass, and even more preferably 20% by mass to 70% by mass, relative to all structural units of the alkali-soluble resin, from the viewpoint of achieving better effects of the present disclosure.
[0134] Furthermore, when the alkali-soluble resin contains a structural unit having an aliphatic hydrocarbon ring structure, the content of the structural unit having an aliphatic hydrocarbon ring structure in the alkali-soluble resin is preferably 5 mol % to 70 mol %, more preferably 10 mol % to 60 mol %, and even more preferably 20 mol % to 50 mol %, relative to all structural units of the alkali-soluble resin, from the viewpoint of achieving better effects of the present disclosure.
[0135] When the alkali-soluble resin contains a structural unit represented by the above formula (Cy), the content of the structural unit represented by the above formula (Cy) in the alkali-soluble resin is, from the viewpoint of achieving better effects of the present disclosure, preferably 5 mol % to 70 mol %, more preferably 10 mol % to 60 mol %, and even more preferably 20 mol % to 50 mol %, relative to all structural units of the alkali-soluble resin.
[0136] When the alkali-soluble resin contains a structural unit having an aromatic ring structure and a structural unit having an aliphatic hydrocarbon ring structure, the total content of the structural units having an aromatic ring structure and the structural units having an aliphatic hydrocarbon ring structure in the alkali-soluble resin is, from the viewpoint of achieving better effects of the present disclosure, preferably 10% by mass to 90% by mass, more preferably 20% by mass to 80% by mass, and even more preferably 40% by mass to 75% by mass, relative to all structural units of the alkali-soluble resin.
[0137] Furthermore, when the alkali-soluble resin contains a structural unit having an aromatic ring structure and a structural unit having an aliphatic hydrocarbon ring structure, the total content of the structural units having an aromatic ring structure and the structural units having an aliphatic hydrocarbon ring structure in the alkali-soluble resin is, from the viewpoint of achieving better effects of the present disclosure, preferably 10 mol % to 80 mol %, more preferably 20 mol % to 70 mol %, and even more preferably 40 mol % to 60 mol %, relative to all structural units of the alkali-soluble resin.
[0138] When the alkali-soluble resin contains a structural unit represented by the above formula (S) and a structural unit represented by the above formula (Cy), the total content of the structural unit represented by the above formula (S) and the structural unit represented by the above formula (Cy) in the alkali-soluble resin is, from the viewpoint of achieving better effects of the present disclosure, preferably 10 mol % to 80 mol %, more preferably 20 mol % to 70 mol %, and even more preferably 40 mol % to 60 mol %, relative to all structural units of the alkali-soluble resin.
[0139] From the viewpoint of achieving superior effects of the present disclosure, the molar amount nS of the structural unit represented by formula (S) in the alkali-soluble resin and the molar amount nCy of the structural unit represented by formula (Cy) preferably satisfy the relationship shown in formula (SCy) below, more preferably satisfy the relationship shown in formula (SCy-1) below, and even more preferably satisfy the relationship shown in formula (SCy-2) below: 0.20≦nS / (nS+nCy)≦0.80...formula (SCy) 0.30≦nS / (nS+nCy)≦0.75...formula (SCy-1) 0.40≦nS / (nS+nCy)≦0.70...formula (SCy-2)
[0140] From the viewpoint of achieving superior effects of the present disclosure, the alkali-soluble resin preferably contains a structural unit having an acid group. Examples of the acid group include a carboxy group, a sulfo group, a phosphonic acid group, and a phosphoric acid group, and the carboxy group is preferred. As the structural unit having an acid group, a structural unit derived from (meth)acrylic acid shown below is preferred, and a structural unit derived from methacrylic acid is more preferred.
[0141]
[0142] When the alkali-soluble resin contains a structural unit having an acid group, it may contain one type of structural unit having an acid group alone, or may contain two or more types of structural units having an acid group.
[0143] When the alkali-soluble resin contains a structural unit having an acid group, the content of the structural unit having an acid group in the alkali-soluble resin is preferably 5% by mass to 50% by mass, more preferably 5% by mass to 40% by mass, and even more preferably 10% by mass to 30% by mass, relative to all structural units of the alkali-soluble resin, from the viewpoint of achieving better effects of the present disclosure.
[0144] From the viewpoint of achieving superior effects of the present disclosure, the content of structural units having an acid group in the alkali-soluble resin is preferably 5 mol % to 70 mol %, more preferably 10 mol % to 50 mol %, and even more preferably 20 mol % to 40 mol %, relative to all structural units of the alkali-soluble resin.
[0145] From the viewpoint of achieving better effects of the present disclosure, the content of the structural units derived from (meth)acrylic acid in the alkali-soluble resin is preferably 5 mol % to 70 mol %, more preferably 10 mol % to 50 mol %, and even more preferably 20 mol % to 40 mol %, relative to all structural units of the alkali-soluble resin.
[0146] From the viewpoint of achieving superior effects of the present disclosure, the alkali-soluble resin preferably has a reactive group, and more preferably contains a structural unit having a reactive group. The reactive group is preferably a radically polymerizable group, and more preferably an ethylenically unsaturated group. Furthermore, when the alkali-soluble resin has an ethylenically unsaturated group, the alkali-soluble resin preferably contains a structural unit having an ethylenically unsaturated group in a side chain. In the present disclosure, the term "main chain" refers to the relatively longest bond chain in the molecule of the polymer compound constituting the resin, and the term "side chain" refers to an atomic group branched from the main chain. The ethylenically unsaturated group is more preferably an allyl group or a (meth)acryloyloxy group. Examples of structural units having a reactive group include, but are not limited to, those shown below.
[0147]
[0148] When the alkali-soluble resin contains a structural unit having a reactive group, it may contain one type of structural unit having a reactive group alone, or may contain two or more types of structural units having a reactive group.
[0149] When the alkali-soluble resin contains a structural unit having a reactive group, the content of the structural unit having a reactive group in the alkali-soluble resin is preferably 5% by mass to 70% by mass, more preferably 10% by mass to 50% by mass, and even more preferably 20% by mass to 40% by mass, relative to all structural units of the alkali-soluble resin, from the viewpoint of achieving better effects of the present disclosure.
[0150] Furthermore, when the alkali-soluble resin contains a structural unit having a reactive group, the content of the structural unit having a reactive group in the alkali-soluble resin is preferably 5 mol % to 70 mol %, more preferably 10 mol % to 60 mol %, and even more preferably 20 mol % to 50 mol %, relative to all structural units of the alkali-soluble resin, from the viewpoint of achieving better effects of the present disclosure.
[0151] Examples of a method for introducing a reactive group into an alkali-soluble resin include a method of reacting a functional group such as a hydroxy group, a carboxy group, a primary amino group, a secondary amino group, an acetoacetyl group, or a sulfo group with a compound such as an epoxy compound, a blocked isocyanate compound, an isocyanate compound, a vinyl sulfone compound, an aldehyde compound, a methylol compound, or a carboxylic acid anhydride.
[0152] A preferred example of a method for introducing a reactive group into an alkali-soluble resin is to synthesize a polymer having a carboxy group by polymerization, and then react some of the carboxy groups of the resulting polymer with glycidyl (meth)acrylate by a polymerization reaction to introduce a (meth)acryloyloxy group into the polymer. This method can produce an alkali-soluble resin having a (meth)acryloyloxy group in its side chain. The polymerization reaction is preferably carried out at a temperature of 70°C to 100°C, more preferably at a temperature of 80°C to 90°C. The polymerization initiator used in the polymerization reaction is preferably an azo-based initiator, and for example, V-601 (trade name) or V-65 (trade name) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. is more preferred. The polymerization reaction is preferably carried out at a temperature of 80°C to 110°C. A catalyst such as an ammonium salt is preferably used in the polymerization reaction.
[0153] As the alkali-soluble resin, the polymers shown below are preferred from the viewpoint of achieving better effects of the present disclosure. Note that the content ratios (a to d) of the respective structural units shown below, the weight average molecular weight Mw, and the like can be appropriately changed depending on the purpose.
[0154]
[0155] The preferred values for the content ratio of the above structural units are as follows: a: 20% by mass to 60% by mass b: 10% by mass to 50% by mass c: 5% by mass to 25% by mass d: 10% by mass to 50% by mass
[0156]
[0157] The preferred values for the content ratio of the above structural units are as follows: a: 20% by mass to 60% by mass b: 10% by mass to 50% by mass c: 5% by mass to 25% by mass d: 10% by mass to 50% by mass
[0158]
[0159] The preferred values for the content ratio of the above structural units are as follows: a: 30% by mass to 65% by mass b: 1% by mass to 20% by mass c: 5% by mass to 25% by mass d: 10% by mass to 50% by mass
[0160]
[0161] The preferred values for the content ratio of the above structural units are as follows: a: 1% by mass to 20% by mass b: 20% by mass to 60% by mass c: 5% by mass to 25% by mass d: 10% by mass to 50% by mass
[0162] The alkali-soluble resin may contain a polymer (hereinafter also referred to as "polymer X") containing a structural unit having a carboxylic acid anhydride structure. The carboxylic acid anhydride structure may be either a chain carboxylic acid anhydride structure or a cyclic carboxylic acid anhydride structure, but is preferably a cyclic carboxylic acid anhydride structure. The ring of the cyclic carboxylic acid anhydride structure is preferably a 5- to 7-membered ring, more preferably a 5- or 6-membered ring, and even more preferably a 5-membered ring.
[0163] The structural unit having a carboxylic acid anhydride structure is preferably a structural unit containing, in its main chain, a divalent group obtained by removing two hydrogen atoms from a compound represented by the following formula P-1, or a structural unit in which a monovalent group obtained by removing one hydrogen atom from a compound represented by the following formula P-1 is bonded to the main chain directly or via a divalent linking group:
[0164]
[0165] In formula P-1, R A1a represents a substituent, n 1a R A1a may be the same or different, Z 1a represents a divalent group forming a ring containing —C(═O)—O—C(═O)—, n 1a represents an integer of 0 or greater.
[0166] R A1a Examples of the substituent represented by the formula include an alkyl group.
[0167] Z 1a As the alkylene group, an alkylene group having 2 to 4 carbon atoms is preferable, an alkylene group having 2 or 3 carbon atoms is more preferable, and an alkylene group having 2 carbon atoms is even more preferable.
[0168] n 1a represents an integer of 0 or more. 1a represents an alkylene group having 2 to 4 carbon atoms, n1a is preferably an integer of 0 to 4, more preferably an integer of 0 to 2, and even more preferably 0.
[0169] n 1a When R represents an integer of 2 or more, there are multiple R A1a may be the same or different. A1a may be bonded to each other to form a ring, but preferably do not bond to each other to form a ring.
[0170] As a structural unit having a carboxylic acid anhydride structure, a structural unit derived from an unsaturated carboxylic acid anhydride is preferred, a structural unit derived from an unsaturated cyclic carboxylic acid anhydride is more preferred, a structural unit derived from an unsaturated aliphatic cyclic carboxylic acid anhydride is even more preferred, a structural unit derived from maleic anhydride or itaconic anhydride is particularly preferred, and a structural unit derived from maleic anhydride is most preferred.
[0171] Specific examples of structural units having a carboxylic acid anhydride structure are listed below, but the structural units having a carboxylic acid anhydride structure are not limited to these specific examples. In the following structural units, Rx represents a hydrogen atom, a methyl group, a CH 2 OH group or CF 3 group, and Me represents a methyl group.
[0172]
[0173]
[0174] The polymer X may contain one type of structural unit having a carboxylic acid anhydride structure, or may contain two or more types of structural units.
[0175] The total content of structural units having a carboxylic acid anhydride structure in polymer X is preferably 0 mol % to 60 mol %, more preferably 5 mol % to 40 mol %, and even more preferably 10 mol % to 35 mol %, based on all structural units of polymer X.
[0176] When the alkali-soluble resin contains a polymer X, it may contain one type of polymer X alone or two or more types of polymer X.
[0177] When the photosensitive composition according to the present disclosure contains polymer X, the content of polymer X in the photosensitive composition is preferably 0.1% by mass to 30% by mass, more preferably 0.2% by mass to 20% by mass, even more preferably 0.5% by mass to 20% by mass, and still more preferably 1% by mass to 20% by mass, relative to the total solid content of the photosensitive composition, from the viewpoint of achieving better effects of the present disclosure.
[0178] From the viewpoint of achieving better effects of the present disclosure, the weight average molecular weight (Mw) of the alkali-soluble resin is preferably 5,000 or more, more preferably 10,000 or more, even more preferably 10,000 to 50,000, and particularly preferably 15,000 to 30,000.
[0179] The acid value of the alkali-soluble resin is preferably 10 mgKOH / g to 200 mgKOH / g, more preferably 60 mgKOH / g to 200 mgKOH / g, even more preferably 60 mgKOH / g to 150 mgKOH / g, and particularly preferably 70 mgKOH / g to 130 mgKOH / g. The acid value of the alkali-soluble resin is a value measured according to the method described in JIS K0070:1992.
[0180] From the viewpoint of developability, the dispersity of the alkali-soluble resin is preferably from 1.0 to 6.0, more preferably from 1.0 to 5.0, even more preferably from 1.0 to 4.0, and particularly preferably from 1.0 to 3.0.
[0181] When the photosensitive composition according to the present disclosure contains an alkali-soluble resin, it may contain one type of alkali-soluble resin alone or two or more types of alkali-soluble resins.
[0182] When the photosensitive composition according to the present disclosure contains an alkali-soluble resin, the content of the alkali-soluble resin in the photosensitive composition is preferably 10% by mass to 90% by mass, more preferably 20% by mass to 80% by mass, and even more preferably 30% by mass to 70% by mass, relative to the total solid content of the photosensitive composition, from the viewpoint of achieving better effects of the present disclosure.
[0183] <Polymerizable Monomer> The photosensitive composition according to the present disclosure may contain a polymerizable monomer. The polymerizable monomer is a monomer having a polymerizable group. Examples of the polymerizable group include a radical polymerizable group and a cation polymerizable group, and the radical polymerizable group is preferred.
[0184] The polymerizable monomer preferably includes a radical polymerizable monomer having an ethylenically unsaturated group, and the ethylenically unsaturated group is preferably a (meth)acryloyloxy group.
[0185] One preferred embodiment of the polymerizable monomer is a compound represented by the following formula (M) (hereinafter also referred to as "compound M"). 2 -R 1 -Q 1 ...Formula (M) In formula (M), Q 1 and Q 2 each independently represents a (meth)acryloyloxy group, R 1 represents a divalent linking group having a chain structure.
[0186] Q in formula (M) 1 and Q 2 From the viewpoint of ease of synthesis, it is preferable that Q in formula (M) are the same group. 1 and Q 2 is preferably an acryloyloxy group from the viewpoint of reactivity.
[0187] R in formula (M) 1 From the viewpoint of achieving superior effects of the present disclosure, the alkylene group may be a hydrocarbon group, an alkyleneoxyalkylene group (-L 1 -O-L 1 -), or a polyalkyleneoxyalkylene group (-(L 1 -O) p -L 1-) is preferred, a hydrocarbon group having 2 to 20 carbon atoms or a polyalkyleneoxyalkylene group is more preferred, an alkylene group having 4 to 20 carbon atoms is even more preferred, and a straight-chain alkylene group having 6 to 18 carbon atoms is particularly preferred. The hydrocarbon group may have a chain structure at least in part, and the portion other than the chain structure is not particularly limited, and may be, for example, a branched, cyclic, or straight-chain alkylene group having 1 to 5 carbon atoms, an arylene group, an ether bond, or a combination thereof, and is preferably an alkylene group or a group combining two or more alkylene groups and one or more arylene groups, more preferably an alkylene group, and even more preferably a straight-chain alkylene group. L 1 each independently represents an alkylene group, preferably an ethylene group, a propylene group, or a butylene group, and more preferably an ethylene group or a 1,2-propylene group. p represents an integer of 2 or more, preferably an integer of 2 to 10.
[0188] Q in formula (M) 1 and Q 2 From the viewpoint of achieving a more excellent effect of the present disclosure, the number of atoms in the shortest linking chain connecting "Q" and "Q" is preferably 3 to 50, more preferably 4 to 40, even more preferably 6 to 20, and particularly preferably 8 to 12. 1 and Q 2 The number of atoms in the shortest chain connecting Q 1 R connected to 1 Q from atoms in 2 R connected to 1 is the shortest number of atoms that connects to the atom in
[0189] Specific examples of compound M include 1,3-butanediol di(meth)acrylate, tetramethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,7-heptanediol di(meth)acrylate, 1,8-octanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, di(meth)acrylate of hydrogenated bisphenol A, di(meth)acrylate of hydrogenated bisphenol F, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, poly(ethylene glycol / propylene glycol) di(meth)acrylate, and polybutylene glycol di(meth)acrylate. The above ester monomers can also be used as a mixture. From the viewpoint of achieving better effects of the present disclosure, compound M is preferably at least one compound selected from the group consisting of 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, and neopentyl glycol di(meth)acrylate, more preferably at least one compound selected from the group consisting of 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, and 1,10-decanediol di(meth)acrylate, and even more preferably at least one compound selected from 1,9-nonanediol di(meth)acrylate and 1,10-decanediol di(meth)acrylate.
[0190] One suitable embodiment of the polymerizable monomer is a difunctional or higher ethylenically unsaturated compound. In the present disclosure, the term "difunctional or higher ethylenically unsaturated compound" refers to a compound having two or more ethylenically unsaturated groups in one molecule. The ethylenically unsaturated group in the ethylenically unsaturated compound is preferably a (meth)acryloyl group. The ethylenically unsaturated compound is preferably a (meth)acrylate compound.
[0191] The difunctional ethylenically unsaturated compound is not particularly limited and can be appropriately selected from known compounds. Examples of the difunctional ethylenically unsaturated compound other than the compound M include tricyclodecane dimethanol di(meth)acrylate, dioxane glycol di(meth)acrylate, and 1,4-cyclohexanediol di(meth)acrylate.
[0192] Commercially available bifunctional ethylenically unsaturated compounds include, for example, tricyclodecane dimethanol diacrylate (trade name: NK Ester A-DCP, manufactured by Shin-Nakamura Chemical Co., Ltd.), tricyclodecane dimenanol dimethacrylate (trade name: NK Ester DCP, manufactured by Shin-Nakamura Chemical Co., Ltd.), 1,9-nonanediol diacrylate (trade name: NK Ester A-NOD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.), 1,6-hexanediol diacrylate (trade name: NK Ester A-HD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.), and dioxane glycol diacrylate (trade name: KAYARAD (registered trademark) R-604, manufactured by Nippon Kayaku Co., Ltd.).
[0193] The tri- or higher functional ethylenically unsaturated compound is not particularly limited and can be appropriately selected from known compounds. Examples of the tri- or higher functional ethylenically unsaturated compound include dipentaerythritol (tri / tetra / penta / hexa)(meth)acrylate, pentaerythritol (tri / tetra)(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, isocyanuric acid (meth)acrylate, and (meth)acrylate compounds having a glycerin tri(meth)acrylate skeleton.
[0194] In the present disclosure, the term "(tri / tetra / penta / hexa)(meth)acrylate" is a concept that encompasses tri(meth)acrylate, tetra(meth)acrylate, penta(meth)acrylate, and hexa(meth)acrylate, and the term "(tri / tetra)(meth)acrylate" is a concept that encompasses tri(meth)acrylate and tetra(meth)acrylate.
[0195] Further, examples of the polymerizable monomer include caprolactone-modified (meth)acrylate compounds (such as KAYARAD (registered trademark) DPCA-20 manufactured by Nippon Kayaku Co., Ltd. and A-9300-1CL manufactured by Shin-Nakamura Chemical Co., Ltd.), alkylene oxide-modified (meth)acrylate compounds (such as KAYARAD (registered trademark) RP-1040 manufactured by Nippon Kayaku Co., Ltd., ATM-35E and A-9300 manufactured by Shin-Nakamura Chemical Co., Ltd., and EBECRYL (registered trademark) 135 manufactured by Daicel-Allnex Corporation), and ethoxylated glycerin triacrylate (such as NK Ester A-GLY-9E manufactured by Shin-Nakamura Chemical Co., Ltd.).
[0196] Examples of polymerizable monomers include urethane (meth)acrylate compounds. Examples of urethane (meth)acrylates include urethane di(meth)acrylates. Examples of urethane di(meth)acrylates include propylene oxide-modified urethane di(meth)acrylates and ethylene oxide and propylene oxide-modified urethane di(meth)acrylates. Examples of urethane (meth)acrylates include trifunctional or higher urethane (meth)acrylates. The lower limit of the number of functional groups is more preferably 6 or more, and even more preferably 8 or more. The upper limit of the number of functional groups is preferably 20 or less.
[0197] Examples of tri- or higher functional urethane (meth)acrylates include 8UX-015A (trade name) manufactured by Taisei Fine Chemical Co., Ltd., UA-32P (trade name), U-15HA (trade name), and UA-1100H (trade name) manufactured by Shin-Nakamura Chemical Co., Ltd., AH-600 (trade name) manufactured by Kyoeisha Chemical Co., Ltd., and UA-306H (trade name), UA-306T (trade name), UA-306I (trade name), UA-510H (trade name), and UX-5000 (trade name) manufactured by Nippon Kayaku Co., Ltd.
[0198] One preferred embodiment of the polymerizable monomer is an ethylenically unsaturated compound having an acid group. Examples of the acid group include a phosphate group, a sulfo group, and a carboxy group. The acid group is preferably a carboxy group.
[0199] Examples of the ethylenically unsaturated compound having an acid group include a tri- or tetrafunctional ethylenically unsaturated compound having an acid group (a compound obtained by introducing a carboxy group into a pentaerythritol tri- or tetraacrylate (PETA) skeleton (acid value: 80 mg KOH / g to 120 mg KOH / g)), a penta- or hexafunctional ethylenically unsaturated compound having an acid group (a compound obtained by introducing a carboxy group into a dipentaerythritol penta- or hexaacrylate (DPHA) skeleton (acid value: 25 mg KOH / g to 70 mg KOH / g)), and the like. A tri- or higher functional ethylenically unsaturated compound having an acid group may be used in combination with a difunctional ethylenically unsaturated compound having an acid group, if necessary.
[0200] The ethylenically unsaturated compound having an acid group is preferably at least one selected from the group consisting of difunctional or higher ethylenically unsaturated compounds having a carboxy group and carboxylic acid anhydrides thereof. When the ethylenically unsaturated compound having an acid group is at least one selected from the group consisting of difunctional or higher ethylenically unsaturated compounds having a carboxy group and carboxylic acid anhydrides thereof, developability and film strength are further improved. The difunctional or higher ethylenically unsaturated compound having a carboxy group is not particularly limited and can be appropriately selected from known compounds. Examples of difunctional or higher ethylenically unsaturated compounds having a carboxy group include ARONIX (registered trademark) TO-2349 (manufactured by Toagosei Co., Ltd.), ARONIX (registered trademark) M-520 (manufactured by Toagosei Co., Ltd.), and ARONIX (registered trademark) M-510 (manufactured by Toagosei Co., Ltd.).
[0201] As the ethylenically unsaturated compound having an acid group, the polymerizable compound having an acid group described in paragraphs
[0025] to
[0030] of JP-A No. 2004-239942 is preferred, and the contents of this publication are incorporated herein by reference.
[0202] Examples of polymerizable monomers include compounds obtained by reacting a polyhydric alcohol with an α,β-unsaturated carboxylic acid, compounds obtained by reacting a glycidyl group-containing compound with an α,β-unsaturated carboxylic acid, urethane monomers such as (meth)acrylate compounds having a urethane bond, phthalic acid compounds such as γ-chloro-β-hydroxypropyl-β'-(meth)acryloyloxyethyl-o-phthalate, β-hydroxyethyl-β'-(meth)acryloyloxyethyl-o-phthalate, and β-hydroxypropyl-β'-(meth)acryloyloxyethyl-o-phthalate, and (meth)acrylic acid alkyl esters. These may be used alone or in combination of two or more.
[0203] Examples of compounds obtained by reacting a polyhydric alcohol with an α,β-unsaturated carboxylic acid include bisphenol A-based (meth)acrylate compounds such as 2,2-bis(4-((meth)acryloyloxypolyethoxy)phenyl)propane, 2,2-bis(4-((meth)acryloyloxypolypropoxy)phenyl)propane, and 2,2-bis(4-((meth)acryloyloxypolyethoxypolypropoxy)phenyl)propane; polyethylene glycol di(meth)acrylates having 2 to 14 ethylene oxide groups; polypropylene glycol di(meth)acrylates having 2 to 14 propylene oxide groups; and polyethylene polypropylene glycol di(meth)acrylates having 2 to 14 ethylene oxide groups and 2 to 14 propylene oxide groups. trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane ethoxy tri(meth)acrylate, trimethylolpropane diethoxy tri(meth)acrylate, trimethylolpropane triethoxy tri(meth)acrylate, trimethylolpropane tetraethoxy tri(meth)acrylate, trimethylolpropane pentaethoxy tri(meth)acrylate, di(trimethylolpropane) tetraacrylate, tetramethylolmethane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate. The compound obtained by reacting a polyhydric alcohol with an α,β-unsaturated carboxylic acid is preferably an ethylenically unsaturated compound having a tetramethylolmethane structure or a trimethylolpropane structure, and more preferably tetramethylolmethane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, trimethylolpropane tri(meth)acrylate, or di(trimethylolpropane)tetraacrylate.
[0204] Examples of the polymerizable monomer include caprolactone-modified ethylenically unsaturated compounds (e.g., KAYARAD (registered trademark) DPCA-20 manufactured by Nippon Kayaku Co., Ltd., and A-9300-1CL manufactured by Shin-Nakamura Chemical Co., Ltd.), alkylene oxide-modified ethylenically unsaturated compounds (e.g., KAYARAD (registered trademark) RP-1040 manufactured by Nippon Kayaku Co., Ltd., ATM-35E and A-9300 manufactured by Shin-Nakamura Chemical Co., Ltd., and EBECRYL (registered trademark) 135 manufactured by Daicel-Allnex Corporation), and ethoxylated glycerin triacrylate (e.g., A-GLY-9E manufactured by Shin-Nakamura Chemical Co., Ltd.).
[0205] As the polymerizable monomer (particularly, an ethylenically unsaturated compound), from the viewpoint of excellent developability of the photosensitive composition layer formed using the photosensitive composition, a polymerizable monomer containing an ester bond is also preferred.The ethylenically unsaturated compound containing an ester bond is not particularly limited as long as it contains an ester bond in the molecule, and from the viewpoint of excellent effects of the present disclosure, an ethylenically unsaturated compound having a tetramethylolmethane structure or a trimethylolpropane structure is preferred, and tetramethylolmethane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, trimethylolpropane tri(meth)acrylate, or di(trimethylolpropane)tetraacrylate is more preferred.
[0206] From the viewpoint of providing reliability, the ethylenically unsaturated compound preferably contains an ethylenically unsaturated compound having an aliphatic group having 6 to 20 carbon atoms and an ethylenically unsaturated compound having a tetramethylolmethane structure or a trimethylolpropane structure. Examples of ethylenically unsaturated compounds having an aliphatic structure having 6 or more carbon atoms include 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, and tricyclodecane dimethanol di(meth)acrylate.
[0207] One suitable embodiment of the polymerizable monomer is a polymerizable compound having an aliphatic hydrocarbon ring structure (preferably a bifunctional ethylenically unsaturated compound). As the polymerizable monomer, a polymerizable compound having a ring structure in which two or more aliphatic hydrocarbon rings are fused (preferably a structure selected from the group consisting of a tricyclodecane structure and a tricyclodecene structure) is preferred, a bifunctional ethylenically unsaturated compound having a ring structure in which two or more aliphatic hydrocarbon rings are fused is more preferred, and tricyclodecane dimethanol di(meth)acrylate is even more preferred. As the aliphatic hydrocarbon ring structure, from the viewpoint of achieving better effects of the present disclosure, a cyclopentane structure, a cyclohexane structure, a tricyclodecane structure, a tricyclodecene structure, a norbornane structure, or an isoborone structure is preferred.
[0208] The molecular weight of the polymerizable monomer is not particularly limited, but is preferably, for example, 200 to 3,000, more preferably 250 to 2,600, even more preferably 280 to 2,200, and particularly preferably 300 to 2,200.
[0209] Among the polymerizable monomers contained in the photosensitive composition according to the present disclosure, the content ratio of polymerizable monomers having a molecular weight of 300 or less is preferably 30 mass % or less, more preferably 25 mass % or less, and even more preferably 20 mass % or less, relative to the content of all polymerizable monomers contained in the photosensitive composition.
[0210] One suitable embodiment of the photosensitive composition according to the present disclosure is an embodiment in which the photosensitive composition contains a difunctional or higher ethylenically unsaturated compound as a polymerizable monomer. The photosensitive composition according to the present disclosure preferably contains a difunctional or higher ethylenically unsaturated compound as a polymerizable monomer, more preferably a trifunctional or higher ethylenically unsaturated compound, and even more preferably a trifunctional or tetrafunctional ethylenically unsaturated compound.
[0211]
[0033] Furthermore, one suitable aspect of the photosensitive composition according to the present disclosure is an aspect in which the photosensitive composition contains, as the polymerizable monomer, a bifunctional ethylenically unsaturated compound having an aliphatic hydrocarbon ring structure, and, as the alkali-soluble resin, a resin having a structural unit having an aliphatic hydrocarbon ring.
[0212] One suitable embodiment of the photosensitive composition according to the present disclosure is an embodiment in which the photosensitive composition contains, as polymerizable monomers, Compound M and an ethylenically unsaturated compound having an acid group. The photosensitive composition according to the present disclosure preferably contains, as polymerizable monomers, Compound M and an ethylenically unsaturated compound having an acid group, more preferably contains, as polymerizable monomers, 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, and a polyfunctional ethylenically unsaturated compound having a carboxylic acid group, and even more preferably contains, as polymerizable monomers, 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, and a succinic acid-modified product of dipentaerythritol pentaacrylate.
[0213]
[0033] Furthermore, one suitable aspect of the photosensitive composition according to the present disclosure is an aspect in which the photosensitive composition contains, as polymerizable monomers, a compound M and an ethylenically unsaturated compound having an acid group, and a thermally crosslinkable compound described below. A more preferred aspect is one in which the photosensitive composition contains, as polymerizable monomers, a compound M and an ethylenically unsaturated compound having an acid group, and a blocked isocyanate compound described below.
[0214]
[0044] Furthermore, one suitable embodiment of the photosensitive composition according to the present disclosure is an embodiment in which the photosensitive composition contains a difunctional ethylenically unsaturated compound (preferably a difunctional (meth)acrylate compound) and a tri- or higher functional ethylenically unsaturated compound (preferably a tri- or higher functional (meth)acrylate compound) from the viewpoints of suppressing development residues and rust prevention.
[0215] When the photosensitive composition according to the present disclosure contains a difunctional ethylenically unsaturated compound and a tri- or higher functional ethylenically unsaturated compound, the mass ratio of the content of the difunctional ethylenically unsaturated compound to the content of the tri- or higher functional ethylenically unsaturated compound is preferably 10:90 to 90:10, and more preferably 30:70 to 70:30.
[0216] The ratio of the content of the bifunctional ethylenically unsaturated compound to the total content of all ethylenically unsaturated compounds is preferably 20% by mass to 80% by mass, more preferably 30% by mass to 70% by mass.
[0217] The content of the bifunctional ethylenically unsaturated compound in the photosensitive composition according to the present disclosure is preferably 10% by mass to 60% by mass, and more preferably 15% by mass to 40% by mass, relative to the total solid content of the photosensitive composition.
[0218] Furthermore, one suitable embodiment of the photosensitive composition according to the present disclosure is an embodiment in which the photosensitive composition contains a compound M and a bifunctional ethylenically unsaturated compound having an aliphatic hydrocarbon ring structure, from the viewpoint of rust prevention.
[0219]
[0033] Furthermore, one suitable aspect of the photosensitive composition according to the present disclosure is an aspect in which the photosensitive composition contains a compound M and an ethylenically unsaturated compound having an acid group, from the viewpoints of substrate adhesion, suppression of development residues, and rust prevention. An aspect in which the photosensitive composition contains a compound M, a bifunctional ethylenically unsaturated compound having an aliphatic hydrocarbon ring structure, and an ethylenically unsaturated compound having an acid group is more preferred, an aspect in which the photosensitive composition contains a compound M, a bifunctional ethylenically unsaturated compound having an aliphatic hydrocarbon ring structure, a tri- or higher functional ethylenically unsaturated compound, and an ethylenically unsaturated compound having an acid group is even more preferred, and an aspect in which the photosensitive composition contains a compound M, a bifunctional ethylenically unsaturated compound having an aliphatic hydrocarbon ring structure, a tri- or higher functional ethylenically unsaturated compound, an ethylenically unsaturated compound having an acid group, and a urethane (meth)acrylate compound is particularly preferred.
[0220] Furthermore, one suitable aspect of the photosensitive composition according to the present disclosure is an aspect in which the photosensitive composition contains 1,9-nonanediol diacrylate and a polyfunctional ethylenically unsaturated compound having a carboxylic acid group, from the viewpoints of substrate adhesion, suppression of development residue, and rust prevention. An aspect in which the photosensitive composition contains 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, and a polyfunctional ethylenically unsaturated compound having a carboxylic acid group is more preferred, an aspect in which the photosensitive composition contains 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, dipentaerythritol hexaacrylate, and an ethylenically unsaturated compound having a carboxylic acid group is even more preferred, and an aspect in which the photosensitive composition contains 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, an ethylenically unsaturated compound having a carboxylic acid group, and a urethane acrylate compound is particularly preferred.
[0221] The photosensitive composition according to the present disclosure may contain a monofunctional ethylenically unsaturated compound as the ethylenically unsaturated compound.
[0222] The content of the di- or higher functional ethylenically unsaturated compound in the ethylenically unsaturated compound is preferably 60% by mass to 100% by mass, more preferably 80% by mass to 100% by mass, and even more preferably 90% by mass to 100% by mass, relative to the total content of all ethylenically unsaturated compounds contained in the photosensitive composition according to the present disclosure.
[0223] When the photosensitive composition according to the present disclosure contains a polymerizable monomer, it may contain one type of polymerizable monomer (particularly, an ethylenically unsaturated compound) alone, or may contain two or more types of polymerizable monomers.
[0224] When the photosensitive composition according to the present disclosure contains a polymerizable monomer, the content of the polymerizable monomer (particularly, an ethylenically unsaturated compound) in the photosensitive composition is preferably 1% by mass to 70% by mass, more preferably 5% by mass to 70% by mass, even more preferably 5% by mass to 60% by mass, and particularly preferably 5% by mass to 50% by mass, relative to the total solid content of the photosensitive composition.
[0225] <Photopolymerization initiator> The photosensitive composition according to the present disclosure may contain a photopolymerization initiator. The photopolymerization initiator is not particularly limited, and a known photopolymerization initiator can be used. The photopolymerization initiator may be a photoradical polymerization initiator.
[0226] Examples of the photopolymerization initiator include a photopolymerization initiator having an oxime ester structure (hereinafter also referred to as an "oxime-based photopolymerization initiator"), a photopolymerization initiator having an α-aminoalkylphenone structure (hereinafter also referred to as an "α-aminoalkylphenone-based photopolymerization initiator"), a photopolymerization initiator having an α-hydroxyalkylphenone structure (hereinafter also referred to as an "α-hydroxyalkylphenone-based polymerization initiator"), a photopolymerization initiator having an acylphosphine oxide structure (hereinafter also referred to as an "acylphosphine oxide-based photopolymerization initiator"), a photopolymerization initiator having an N-phenylglycine structure (hereinafter also referred to as an "N-phenylglycine-based photopolymerization initiator"), and a photopolymerization initiator having a hexaarylbiimidazole structure (hereinafter also referred to as a "hexaarylbiimidazole-based photopolymerization initiator").
[0227] The photopolymerization initiator preferably contains at least one selected from the group consisting of an oxime-based photopolymerization initiator, an α-aminoalkylphenone-based photopolymerization initiator, an α-hydroxyalkylphenone-based polymerization initiator, an N-phenylglycine-based photopolymerization initiator, and a hexaarylbiimidazole-based photopolymerization initiator, and more preferably contains at least one selected from the group consisting of an oxime-based photopolymerization initiator, an α-aminoalkylphenone-based photopolymerization initiator, an N-phenylglycine-based photopolymerization initiator, and a hexaarylbiimidazole-based photopolymerization initiator.
[0228] As the photopolymerization initiator, for example, the polymerization initiators described in paragraphs
[0031] to
[0042] of JP-A No. 2011-95716 and paragraphs
[0064] to
[0081] of JP-A No. 2015-014783 may be used.
[0229] Commercially available photopolymerization initiators include 1-[4-(phenylthio)phenyl]-1,2-octanedione-2-(O-benzoyloxime) [trade name: IRGACURE (registered trademark) OXE-01, manufactured by BASF], 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone-1-(O-acetyloxime) [trade name: IRGACURE (registered trademark) OXE-02, manufactured by BASF Corporation], IRGACURE (registered trademark) OXE03 (manufactured by BASF Corporation), IRGACURE (registered trademark) OXE04 (manufactured by BASF Corporation), 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone (trade name: Omnirad (registered trademark) 379EG, manufactured by IGM Resins B.V.), 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one (trade name: Omnirad (registered trademark) 907, manufactured by IGM Resins B.V.) IGM Resins B.V], 2-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}-2-methylpropan-1-one [trade name: Omnirad (registered trademark) 127, IGM Resins B.V], 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone-1 [trade name: Omnirad (registered trademark) 369, IGM Resins B.V], 2-hydroxy-2-methyl-1-phenylpropan-1-one [trade name: Omnirad (registered trademark) 1173, IGM Resins B.V], 1-hydroxycyclohexyl phenyl ketone [trade name: Omnirad (registered trademark) 184, IGM Resins B.V] 2,2-dimethoxy-1,2-diphenylethan-1-one [trade name: Omnirad (registered trademark) 651, manufactured by IGM Resins B.V.], oxime ester type [trade name: Lunar (registered trademark) 6, manufactured by DKSH Japan Co., Ltd.], 1-[4-(phenylthio)phenyl]-3-cyclopentylpropane-1,2-dione-2-(O-benzoyloxime) [trade name: TR-PBG-305, manufactured by Changzhou Strong Electronic New Materials Co., Ltd.], 1,2-propanedione, 3-cyclohexyl-1-[9-ethyl-6-(2-furanylcarbonyl)-9H-carbazol-3-yl]-,2-(O-acetyloxime) [trade name: TR-PBG-326, manufactured by Changzhou Powerful Electronic New Materials Co., Ltd.], 3-cyclohexyl-1-(6-(2-(benzoyloxyimino)hexanoyl)-9-ethyl-9H-carbazol-3-yl)-propane-1,2-dione-2-(O-benzoyloxime) [trade name: TR-PBG-391, manufactured by Changzhou Powerful Electronic New Materials Co., Ltd.], 1-(biphenyl-4-yl)-2-methyl-2-morpholinopropan-1-one [trade name: APi-307, manufactured by Shenzhen UV-ChemTech Ltd.], 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, and the like.
[0230] When the photosensitive composition according to the present disclosure contains a photopolymerization initiator, it may contain one type of photopolymerization initiator alone or two or more types. When the photosensitive composition according to the present disclosure contains two or more types of photopolymerization initiators, it preferably contains an oxime-based photopolymerization initiator or a hexaarylbiimidazole-based photopolymerization initiator and at least one selected from the group consisting of an α-aminoalkylphenone-based photopolymerization initiator and an α-hydroxyalkylphenone-based polymerization initiator.
[0231] When the photosensitive composition according to the present disclosure contains a photopolymerization initiator, the content of the photopolymerization initiator in the photosensitive composition is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1.0% by mass or more, based on the total solid content of the photosensitive composition. The upper limit of the content of the photopolymerization initiator in the photosensitive composition according to the present disclosure is preferably 10% by mass or less, more preferably 5% by mass or less, based on the total solid content of the photosensitive composition.
[0232] <Sensitizer> The photosensitive composition according to the present disclosure may contain a sensitizer. The sensitizer has the effect of further improving the sensitivity of the photopolymerization initiator to actinic rays and suppressing the polymerization inhibition of the polymerizable compound caused by oxygen.
[0233] Examples of sensitizers include triethanolamine, p-dimethylaminobenzoic acid ethyl ester, p-formyldimethylaniline, p-methylthiodimethylaniline, N-phenylglycine, tributyltin acetate, and trithiane.
[0234] When the photosensitive composition according to the present disclosure contains a sensitizer, it may contain one type of sensitizer alone or two or more types of sensitizers.
[0235] When the photosensitive composition according to the present disclosure contains a sensitizer, the content of the sensitizer in the photosensitive composition is preferably 0.01% by mass to 1% by mass, and more preferably 0.02% by mass to 0.5% by mass, relative to the total solid content of the photosensitive composition.
[0236] <Heterocyclic Compound> The photosensitive composition according to the present disclosure may contain a heterocyclic compound. The heterocycle contained in the heterocyclic compound may be either a monocyclic or polycyclic heterocycle. Examples of heteroatoms contained in the heterocyclic compound include a nitrogen atom, an oxygen atom, and a sulfur atom. The heterocyclic compound preferably contains at least one atom selected from the group consisting of a nitrogen atom, an oxygen atom, and a sulfur atom, and more preferably contains a nitrogen atom.
[0237] Examples of heterocyclic compounds include triazole compounds, benzotriazole compounds, tetrazole compounds, thiadiazole compounds, triazine compounds, rhodanine compounds, thiazole compounds, benzothiazole compounds, benzimidazole compounds, benzoxazole compounds, and pyrimidine compounds. The heterocyclic compound is preferably at least one compound selected from the group consisting of triazole compounds, benzotriazole compounds, tetrazole compounds, thiadiazole compounds, triazine compounds, rhodanine compounds, thiazole compounds, benzothiazole compounds, benzimidazole compounds, and benzoxazole compounds, and more preferably at least one compound selected from the group consisting of triazole compounds, benzotriazole compounds, tetrazole compounds, thiadiazole compounds, thiazole compounds, benzothiazole compounds, benzimidazole compounds, and benzoxazole compounds.
[0238] Preferred specific examples of the heterocyclic compound are shown below.
[0239] Examples of triazole compounds and benzotriazole compounds include the following compounds.
[0240]
[0241]
[0242] Examples of the tetrazole compound include the following compounds.
[0243]
[0244]
[0245] Examples of the thiadiazole compound include the following compounds:
[0246]
[0247] Examples of the triazine compound include the following compounds:
[0248]
[0249] Examples of rhodanine compounds include the following compounds:
[0250]
[0251] Examples of the thiazole compound include the following compounds:
[0252]
[0253] Examples of the benzothiazole compound include the following compounds:
[0254]
[0255] Examples of the benzimidazole compound include the following compounds:
[0256]
[0257]
[0258] Examples of the benzoxazole compound include the following compounds:
[0259]
[0260] When the photosensitive composition according to the present disclosure contains a heterocyclic compound, it may contain one type of heterocyclic compound alone or two or more types of heterocyclic compounds.
[0261] When the photosensitive composition according to the present disclosure contains a heterocyclic compound, the content of the heterocyclic compound in the photosensitive composition is preferably 0.01% by mass to 20.0% by mass, more preferably 0.1% by mass to 10.0% by mass, even more preferably 0.3% by mass to 8.0% by mass, and particularly preferably 0.5% by mass to 5.0% by mass, relative to the total solid content of the photosensitive composition.
[0262] <Aliphatic Thiol Compound> The photosensitive composition according to the present disclosure may contain an aliphatic thiol compound. When the photosensitive composition according to the present disclosure contains an aliphatic thiol compound, the aliphatic thiol compound undergoes an ene-thiol reaction with the radical polymerizable compound having an ethylenically unsaturated group, thereby suppressing cure shrinkage of the resulting film and alleviating stress in the film.
[0263] The aliphatic thiol compound is preferably a monofunctional aliphatic thiol compound or a polyfunctional aliphatic thiol compound (i.e., a bifunctional or higher functional aliphatic thiol compound).
[0264] As the aliphatic thiol compound, a polyfunctional aliphatic thiol compound is preferred from the viewpoint of the adhesion of the formed pattern (particularly the adhesion after exposure). In the present disclosure, the term "polyfunctional aliphatic thiol compound" refers to an aliphatic compound having two or more thiol groups (also referred to as "mercapto groups") in the molecule.
[0265] The polyfunctional aliphatic thiol compound is preferably a low molecular weight compound having a molecular weight of at least 100. Specifically, the molecular weight of the polyfunctional aliphatic thiol compound is more preferably 100 to 1,500, and even more preferably 150 to 1,000.
[0266] The number of functional groups of the polyfunctional aliphatic thiol compound is preferably 2 to 10, more preferably 2 to 8, and even more preferably 2 to 6, from the viewpoint of the adhesion of the pattern to be formed.
[0267] Examples of polyfunctional aliphatic thiol compounds include trimethylolpropane tris(3-mercaptobutyrate), 1,4-bis(3-mercaptobutyryloxy)butane, pentaerythritol tetrakis(3-mercaptobutyrate), 1,3,5-tris(3-mercaptobutyryloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, trimethylolethane tris(3-mercaptobutyrate), tris[(3-mercaptopropionyloxy)ethyl]isocyanurate, trimethylolpropane tris(3-mercaptopropionyloxy)ethyl ester), pentaerythritol tetrakis(3-mercaptopropionate), tetraethylene glycol bis(3-mercaptopropionate), dipentaerythritol hexakis(3-mercaptopropionate), ethylene glycol bisthiopropionate, 1,4-bis(3-mercaptobutyryloxy)butane, 1,2-ethanedithiol, 1,3-propanedithiol, 1,6-hexamethylenedithiol, 2,2′-(ethylenedithio)diethanethiol, meso-2,3-dimercaptosuccinic acid, and di(mercaptoethyl)ether.
[0268] The polyfunctional aliphatic thiol compound is preferably at least one compound selected from the group consisting of trimethylolpropane tris(3-mercaptobutyrate), 1,4-bis(3-mercaptobutyryloxy)butane, and 1,3,5-tris(3-mercaptobutyryloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione.
[0269] Examples of monofunctional aliphatic thiol compounds include 1-octanethiol, 1-dodecanethiol, β-mercaptopropionic acid, methyl-3-mercaptopropionate, 2-ethylhexyl-3-mercaptopropionate, n-octyl-3-mercaptopropionate, methoxybutyl-3-mercaptopropionate, and stearyl-3-mercaptopropionate.
[0270] When the photosensitive composition according to the present disclosure contains an aliphatic thiol compound, it may contain one type of aliphatic thiol compound alone, or may contain two or more types of aliphatic thiol compounds.
[0271] When the photosensitive composition according to the present disclosure contains an aliphatic thiol compound, the content of the aliphatic thiol compound in the photosensitive composition is preferably 5% by mass or more, more preferably 5% by mass to 50% by mass, even more preferably 5% by mass to 30% by mass, and particularly preferably 8% by mass to 20% by mass, relative to the total solid content of the photosensitive composition.
[0272]
[0033] <Thermal Crosslinkable Compound> The photosensitive composition according to the present disclosure preferably contains a thermal crosslinkable compound from the viewpoints of the strength of the cured film obtained and the adhesiveness of the uncured film obtained. Note that, in the present disclosure, a thermal crosslinkable compound having an ethylenically unsaturated group, which will be described later, is not considered an ethylenically unsaturated compound but is considered a thermal crosslinkable compound.
[0273] Examples of the thermally crosslinkable compound include epoxy compounds, oxetane compounds, methylol compounds, and blocked isocyanate compounds. Among these, blocked isocyanate compounds are preferred as the thermally crosslinkable compound from the viewpoints of the strength of the resulting cured film and the adhesiveness of the resulting uncured film.
[0274] Since blocked isocyanate compounds react with hydroxy groups and carboxy groups, for example, when at least one of an alkali-soluble resin and a radically polymerizable compound having an ethylenically unsaturated group has at least one of a hydroxy group and a carboxy group, the hydrophilicity of the formed film tends to decrease and its function as a protective film tends to be enhanced. Note that the term "blocked isocyanate compound" refers to "a compound having a structure in which the isocyanate group of an isocyanate is protected (so-called masked) with a blocking agent."
[0275] The dissociation temperature of the blocked isocyanate compound is not particularly limited, but is preferably 90°C to 160°C, and more preferably 100°C to 150°C. The dissociation temperature of the blocked isocyanate means "the temperature of the endothermic peak associated with the deprotection reaction of the blocked isocyanate when measured by DSC (Differential Scanning Calorimetry) analysis using a differential scanning calorimeter." As the differential scanning calorimeter, for example, a differential scanning calorimeter (Model: DSC6200) manufactured by Seiko Instruments Inc. can be suitably used. However, the differential scanning calorimeter is not limited to this.
[0276] Examples of blocking agents having a dissociation temperature of 90°C to 160°C include active methylene compounds [e.g., malonic acid diesters (dimethyl malonate, diethyl malonate, di-n-butyl malonate, di-2-ethylhexyl malonate, etc.)] and oxime compounds [e.g., compounds having a structure represented by -C(=N-OH)- in the molecule, such as formaldoxime, acetaldoxime, acetoxime, methyl ethyl ketoxime, and cyclohexanone oxime]. From the viewpoint of storage stability, the blocking agent having a dissociation temperature of 90°C to 160°C is preferably at least one compound selected from the group consisting of oxime compounds and pyrazole compounds.
[0277] The blocked isocyanate compound preferably has an isocyanurate structure, for example, from the viewpoint of improving the brittleness of the film and improving adhesion to the transfer target. Blocked isocyanurate compounds having an isocyanurate structure can be obtained, for example, by protecting hexamethylene diisocyanate through isocyanuration. Among blocked isocyanate compounds having an isocyanurate structure, compounds having an oxime structure in which an oxime compound is used as a blocking agent are preferred because they can more easily adjust the dissociation temperature to a preferred range and can easily reduce development residues compared to compounds not having an oxime structure.
[0278] The blocked isocyanate compound may have a polymerizable group. The polymerizable group is not particularly limited, and known polymerizable groups can be used, with a radical polymerizable group being preferred. Examples of the polymerizable group include ethylenically unsaturated groups such as (meth)acryloyloxy groups, (meth)acrylamide groups, and styryl groups, and groups having an epoxy group such as glycidyl groups. The polymerizable group is preferably an ethylenically unsaturated group, more preferably a (meth)acryloyloxy group, and even more preferably an acryloyloxy group.
[0279] Commercially available blocked isocyanate compounds can be used. Examples of commercially available blocked isocyanate compounds include Karenz (registered trademark) AOI-BM, Karenz (registered trademark) MOI-BM, and Karenz (registered trademark) MOI-BP (all manufactured by Showa Denko K.K.), and the blocked Duranate series (for example, Duranate (registered trademark) TPA-B80E, Duranate (registered trademark) SBN-70D, and Duranate (registered trademark) WT32-B75P, manufactured by Asahi Kasei Chemicals Corporation).
[0280] From the viewpoint of achieving superior effects of the present disclosure, it is preferable that the photosensitive composition according to the present disclosure contain a blocked isocyanate compound having an NCO value of 4.5 mmol / g or more (hereinafter also referred to as the "specific blocked isocyanate compound"). The NCO value of the specific blocked isocyanate compound is preferably 5.0 mmol / g or more, and more preferably 5.3 mmol / g or more. From the viewpoint of achieving superior effects of the present disclosure, the upper limit of the NCO value of the specific blocked isocyanate compound is preferably 8.0 mmol / g or less, more preferably 6.0 mmol / g or less, even more preferably 5.8 mmol / g or less, and particularly preferably 5.7 mmol / g or less. The NCO value of the blocked isocyanate compound according to the present disclosure refers to the number of moles of isocyanate groups contained per gram of the blocked isocyanate compound, and is a value calculated from the structural formula of the blocked isocyanate compound.
[0281]
[0033] From the viewpoint of achieving superior effects of the present disclosure, the specific blocked isocyanate compound preferably has a ring structure. Examples of the ring structure include an aliphatic hydrocarbon ring, an aromatic hydrocarbon ring, and a heterocycle. From the viewpoint of achieving superior effects of the present disclosure, an aliphatic hydrocarbon ring and an aromatic hydrocarbon ring are preferred, and an aliphatic hydrocarbon ring is more preferred.
[0282] Examples of the aliphatic hydrocarbon ring include a cyclopentane ring and a cyclohexane ring, with a cyclohexane ring being preferred.
[0283] Examples of the aromatic hydrocarbon ring include a benzene ring and a naphthalene ring, with a benzene ring being preferred.
[0284] An example of the heterocyclic ring is an isocyanurate ring.
[0285] When the specific blocked isocyanate compound has a ring structure, from the viewpoint of achieving better effects of the present disclosure, the number of rings is preferably 1 or 2, and more preferably 1. When the specific blocked isocyanate compound contains a fused ring, the number of rings constituting the fused ring is counted; for example, the number of rings in a naphthalene ring is counted as 2.
[0286] The number of blocked isocyanate groups contained in the specific blocked isocyanate compound is preferably 2 to 5, more preferably 2 or 3, and even more preferably 2, from the viewpoint of achieving excellent strength in the pattern to be formed and achieving better effects of the present disclosure.
[0287] From the viewpoint of achieving superior effects of the present disclosure, the specific blocked isocyanate compound is preferably a blocked isocyanate compound represented by the following formula (Q): 1 -A 1 -L 1 -A 2 -B 2 ...Formula (Q)
[0288] In formula (Q), B 1 and B 2 each independently represents a blocked isocyanate group. 1 and B 2The blocked isocyanate group represented by the formula (I) is not particularly limited, but from the viewpoint of achieving better effects of the present disclosure, it is preferably a group in which the isocyanate group is blocked with an oxime compound, and more preferably a group in which the isocyanate group is blocked with methyl ethyl ketoxime (specifically, *-NH-C(=O)-O-N=C(CH 3 )-C 2 H 5 A group represented by *. 1 or A 2 It is more preferable that B 1 and B 2 are preferably the same group.
[0289] In formula (Q), A 1 and A 2 each independently represents a single bond or an alkylene group having 1 to 10 carbon atoms, and preferably an alkylene group having 1 to 10 carbon atoms. 1 and A 2 The alkylene group represented by the formula (I) may be linear, branched, or cyclic, and is preferably linear. The number of carbon atoms in the alkylene group is 1 to 10, but from the viewpoint of achieving better effects of the present disclosure, it is preferably 1 to 5, more preferably 1 to 3, and even more preferably 1. 1 and A 2 are preferably the same group.
[0290] In formula (Q), L 1represents a divalent linking group. Specific examples of the divalent linking group include divalent hydrocarbon groups. Specific examples of the divalent hydrocarbon group include divalent saturated hydrocarbon groups, divalent aromatic hydrocarbon groups, and groups formed by linking two or more of these groups. The divalent saturated hydrocarbon group may be linear, branched, or cyclic, and is preferably cyclic from the viewpoint of achieving superior effects of the present disclosure. The number of carbon atoms in the divalent saturated hydrocarbon group is preferably 4 to 15, more preferably 5 to 10, and even more preferably 5 to 8, from the viewpoint of achieving superior effects of the present disclosure. The divalent aromatic hydrocarbon group preferably has 5 to 20 carbon atoms. Examples of the divalent aromatic hydrocarbon group include a phenylene group. The divalent aromatic hydrocarbon group may have a substituent (e.g., an alkyl group). The divalent linking group is preferably a linear, branched, or cyclic divalent saturated hydrocarbon group having 5 to 10 carbon atoms, a group in which a cyclic saturated hydrocarbon group having 5 to 10 carbon atoms is linked to a linear alkylene group having 1 to 3 carbon atoms, a divalent aromatic hydrocarbon group which may have a substituent, or a group in which a divalent aromatic hydrocarbon group is linked to a linear alkylene group having 1 to 3 carbon atoms, more preferably a cyclic divalent saturated hydrocarbon group having 5 to 10 carbon atoms or a phenylene group which may have a substituent, still more preferably a cyclohexylene group or a phenylene group which may have a substituent, and particularly preferably a cyclohexylene group.
[0291] From the viewpoint of achieving superior effects of the present disclosure, the blocked isocyanate compound represented by formula (Q) is particularly preferably a blocked isocyanate compound represented by the following formula (QA): 1a -A 1a -L 1a -A 2a -B 2a ...Formula (QA)
[0292] In formula (QA), B 1a and B 2a each independently represents a blocked isocyanate group. 1a and B 2a A preferred embodiment of the formula (Q) is B 1 and B 2is the same as:
[0293] In formula (QA), A 1a and A 2a each independently represents a divalent linking group. 1a and A 2a A preferred embodiment of the divalent linking group in formula (Q) is 1 and A 2 is the same as:
[0294] In formula (QA), L 1a represents a cyclic divalent saturated hydrocarbon group or a divalent aromatic hydrocarbon group. 1a The number of carbon atoms in the cyclic divalent saturated hydrocarbon group in L is preferably 5 to 10, more preferably 5 to 8, even more preferably 5 or 6, and particularly preferably 6. 1a A preferred embodiment of the divalent aromatic hydrocarbon group in formula (Q) is 1 It is the same as L 1a is preferably a cyclic divalent saturated hydrocarbon group, more preferably a cyclic divalent saturated hydrocarbon group having 5 to 10 carbon atoms, even more preferably a cyclic divalent saturated hydrocarbon group having 5 to 10 carbon atoms, particularly preferably a cyclic divalent saturated hydrocarbon group having 5 or 6 carbon atoms, and most preferably a cyclohexylene group. 1a is a cyclohexylene group, the blocked isocyanate compound represented by formula (QA) may be an isomer mixture of cis and trans isomers. The mass ratio of the cis to trans isomers is preferably cis / trans=10 / 90 to 90 / 10, and more preferably cis / trans=40 / 60 to 60 / 40.
[0295] Specific examples of the specific blocked isocyanate compound are shown below, but the specific blocked isocyanate compound is not limited to these.
[0296]
[0297] When the photosensitive composition according to the present disclosure contains a thermally crosslinkable compound, it may contain one type of thermally crosslinkable compound alone, or may contain two or more types of thermally crosslinkable compounds.
[0298] When the photosensitive composition according to the present disclosure contains a thermally crosslinkable compound, the content of the thermally crosslinkable compound in the photosensitive composition is preferably 1% by mass to 50% by mass, and more preferably 5% by mass to 30% by mass, relative to the total solid content of the photosensitive composition.
[0299] The photosensitive composition according to the present disclosure may contain a surfactant. Examples of the surfactant include those described in paragraph
[0017] of Japanese Patent No. 4502784 and paragraphs
[0060] to
[0071] of JP-A-2009-237362.
[0300] Examples of surfactants include hydrocarbon surfactants, fluorine surfactants, and silicone surfactants. From the viewpoint of improving environmental friendliness, it is preferable that the surfactant does not contain a fluorine atom. The surfactant is preferably a hydrocarbon surfactant or a silicone surfactant.
[0301] Commercially available fluorine-based surfactants include, for example, Megafac (registered trademark) F-171, F-172, F-173, F-176, F-177, F-141, F-142, F-143, F-144, F-437, F-475, F-477, F-479, F-482, F-551-A, F-552, F-554, F-555-A, F-556, F-557, F-558, F-559, F-560, F-561, F-563, F-565, F-568, F-575, F-780, EXP.MFS-330, EXP.MFS-578, EXP.MFS-578-2, EXP.MFS-330 ... MFS-579, EXP. MFS-586, EXP. MFS-587, EXP. MFS-628, EXP. MFS-631, EXP. MFS-603, R-01, R-40, R-40-LM, R-41, R-41-LM, RS-43, TF-1956, RS-72-K, RS-90, R-94, and DS-21 (all manufactured by DIC Corporation), Fluorard (registered trademark) FC430, FC431, and FC171 (all manufactured by Sumitomo 3M Limited), Surflon (registered trademark) S-382, SC-101, SC-103, SC-104, SC-105, SC-1068, SC-381, SC-383, S-393, and KH-40 (all manufactured by AGC Inc.), PolyFox (registered trademark) Examples of suitable fluororesin include PF636, PF656, PF6320, PF6520, and PF7002 (manufactured by OMNOVA), Futergent (registered trademark) 710FL, 710FM, 610FM, 601AD, 601ADH2, 602A, 215M, 245F, 251, 212M, 250, 209F, 222F, 208G, 710LA, 710FS, 730LM, 650AC, 681, and 683 (manufactured by NEOS Corporation), and U-120E (manufactured by Unichem Co., Ltd.).
[0302] As the fluorosurfactant, an acrylic compound having a molecular structure with a functional group containing a fluorine atom, which cleaves the functional group containing a fluorine atom when heated, causing the fluorine atom to volatilize, can also be suitably used. Examples of such fluorosurfactants include the Megafac (registered trademark) DS series manufactured by DIC Corporation [The Chemical Daily (February 22, 2016), The Nikkei Business Daily (February 23, 2016)], and a specific example is Megafac (registered trademark) DS-21.
[0303] As the fluorine-based surfactant, it is also preferable to use a polymer of a fluorine atom-containing vinyl ether compound having a fluorinated alkyl group or a fluorinated alkylene ether group and a hydrophilic vinyl ether compound.
[0304] As the fluorine-based surfactant, a block polymer can also be used.
[0305] As the fluorine-based surfactant, a fluorine-containing polymer compound containing a constituent unit derived from a (meth)acrylate compound having a fluorine atom and a constituent unit derived from a (meth)acrylate compound having two or more (preferably, five or more) alkyleneoxy groups (preferably, ethyleneoxy groups or propyleneoxy groups) can also be preferably used.
[0306] As the fluorosurfactant, a fluorine-containing polymer having an ethylenically unsaturated bond-containing group in the side chain can also be used, such as Megafac (registered trademark) RS-101, RS-102, RS-718K, and RS-72-K (all manufactured by DIC Corporation).
[0307] As the fluorine-based surfactant, from the viewpoint of improving environmental compatibility, surfactants derived from alternative materials to compounds having a linear perfluoroalkyl group having 7 or more carbon atoms, such as perfluorooctanoic acid (PFOA) and perfluorooctanesulfonic acid (PFOS), are preferred.
[0308] Examples of hydrocarbon surfactants include glycerol, trimethylolpropane, trimethylolethane, and their ethoxylates and propoxylates (e.g., glycerol propoxylate and glycerol ethoxylate), polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene nonylphenyl ether, polyethylene glycol dilaurate, polyethylene glycol distearate, and sorbitan fatty acid esters.
[0309] Commercially available hydrocarbon surfactants include, for example, Pluronic (registered trademark) L10, L31, L61, L62, 10R5, 17R2, and 25R2, Tetronic (registered trademark) 304, 701, 704, 901, 904, and 150R1, HYDROPALAT (registered trademark) WE 3323 (all manufactured by BASF), Solsperse (registered trademark) 20000 (all manufactured by Lubrizol Japan Co., Ltd.), NCW-101, NCW-1001, and NCW-1002 (all manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), Paionin (registered trademark) D-1105, D-6112, D-6112-W, and D-6315 (all manufactured by Takemoto Oil & Fat Co., Ltd.), and Olfine (registered trademark). E1010, and Surfynol (registered trademark) 104, 400, and 440 (all manufactured by Nissin Chemical Industry Co., Ltd.).
[0310] Examples of silicone surfactants include linear polymers consisting of siloxane bonds, modified siloxane polymers with organic groups introduced into the side chains or terminals, and polymers having a structural unit with a hydrophilic group in the side chain and a structural unit with a siloxane bond-containing group in the side chain.Preferred silicone surfactants are polymers having a structural unit with a hydrophilic group in the side chain and a structural unit with a siloxane bond-containing group in the side chain.The polymer may be a random copolymer or a block copolymer.
[0311] Examples of the structural unit having a hydrophilic group in the side chain include structural units derived from monomers represented by the following formula:
[0312]
[0313] In the formula, R 4 represents a hydrogen atom or a methyl group, R 5 represents a hydrogen atom or a methyl group, n represents an integer of 1 to 4, and m represents an integer of 1 to 100.
[0314] Examples of the structural unit having a siloxane bond-containing group in the side chain include structural units derived from monomers represented by the following formula:
[0315]
[0316] In the formula, each R independently represents an alkyl group having 1 to 3 carbon atoms, and R 1 represents a hydrogen atom or a methyl group, L 1 represents a divalent organic group or a single bond.
[0317] Examples of the structural unit having a siloxane bond-containing group in the side chain include structural units derived from monomers represented by the following formula:
[0318]
[0319] In the formula, R 1 represents a hydrogen atom or a methyl group, R 2 represents an alkylene group having 1 to 10 carbon atoms, and R 3 represents an alkyl group having 1 to 4 carbon atoms, and n represents an integer of 5 to 50.
[0320] Commercially available silicone surfactants include, for example, EXP. S-309-2, EXP. S-315, EXP. S-324, EXP. S-503-2, EXP. S-506, and EXP. S-505-2 (all manufactured by DIC Corporation), DOWSIL (registered trademark) 8032 ADDITIVE, Toray Silicone DC3PA, Toray Silicone SH7PA, Toray Silicone DC11PA, Toray Silicone SH21PA, Toray Silicone SH28PA, Toray Silicone SH29PA, Toray Silicone SH30PA, and Toray Silicone. SH8400 (manufactured by Dow Corning Toray Co., Ltd.), X-22-4952, X-22-4272, X-22-6266, KF-351A, K354L, KF-355A, KF-945, KF-640, KF-642, KF-643, X-22-6191, X-22-4515, KF-6004, KF-6001, KF- 6002, KP-101KP-103, KP-104, KP-105, KP-106, KP-109, KP-109, KP-112, KP-120, KP-12 1, KP-124, KP-125, KP-301, KP-306, KP-310, KP-322, KP-323, KP-327, KP-341, KP-368, K P-369, KP-611, KP-620, KP-621, KP-626, and KP-652 (all manufactured by Shin-Etsu Chemical Co., Ltd.), F-4440, TSF-4300, TSF-4445, TSF-4460, and TSF-4452 (all manufactured by Momentive Performance Materials), and BYK300, BYK 306, BYK307, BYK310, BYK313, BYK315N, BYK320, BYK323, BYK325, BYK330, BYK331, BYK333, BYK345, BYK347, BYK348, BYK349, BYK370, BYK377, and BYK378 (all manufactured by BYK-Chemie).
[0321] The surfactant is preferably a nonionic surfactant.
[0322] When the photosensitive composition according to the present disclosure contains a surfactant, it may contain one type of surfactant alone or two or more types of surfactants.
[0323] When the photosensitive composition according to the present disclosure contains a surfactant, the content of the surfactant in the photosensitive composition is preferably 0.01% by mass to 3.0% by mass, more preferably 0.01% by mass to 1.0% by mass, and even more preferably 0.05% by mass to 0.80% by mass, relative to the total solid content of the photosensitive composition.
[0324] <Polymerization inhibitor> The photosensitive composition according to the present disclosure may contain a polymerization inhibitor. The polymerization inhibitor refers to a compound having the function of delaying or inhibiting a polymerization reaction. The polymerization inhibitor is not particularly limited, and for example, a known compound used as a polymerization inhibitor can be used.
[0325] Examples of the polymerization inhibitor include phenothiazine compounds such as phenothiazine, bis-(1-dimethylbenzyl)phenothiazine, and 3,7-dioctylphenothiazine; bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionic acid][ethylenebis(oxyethylene)]2,4-bis[(laurylthio)methyl]-o-cresol, 1,3,5-tris(3,5-di-t-butyl-4-hydroxybenzyl), 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl), 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, and pentaerythritol tetrakis 3-(3,5-di-te nitroso compounds or salts thereof such as 4-nitrosophenol, N-nitrosodiphenylamine, N-nitrosocyclohexylhydroxylamine, and N-nitrosophenylhydroxylamine; quinone compounds such as methylhydroquinone, t-butylhydroquinone, 2,5-di-t-butylhydroquinone, and 4-benzoquinone; phenol compounds such as 4-methoxyphenol, 4-methoxy-1-naphthol, and t-butylcatechol; and metal salt compounds such as copper dibutyldithiocarbamate, copper diethyldithiocarbamate, manganese diethyldithiocarbamate, and manganese diphenyldithiocarbamate. As the polymerization inhibitor, from the viewpoint of achieving better effects of the present disclosure, at least one selected from the group consisting of a phenothiazine compound, a nitroso compound or a salt thereof, and a hindered phenol compound is preferred, and at least one selected from the group consisting of phenothiazine, bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionic acid], [ethylenebis(oxyethylene)]2,4-bis[(laurylthio)methyl]-o-cresol, 1,3,5-tris(3,5-di-t-butyl-4-hydroxybenzyl), p-methoxyphenol, and N-nitrosophenylhydroxylamine aluminum salt is more preferred.
[0326] When the photosensitive composition according to the present disclosure contains a polymerization inhibitor, it may contain one type of polymerization inhibitor alone or two or more types of polymerization inhibitors.
[0327] When the photosensitive composition according to the present disclosure contains a polymerization inhibitor, the content of the polymerization inhibitor in the photosensitive composition is preferably 0.001% by mass to 5.0% by mass, more preferably 0.01% by mass to 3.0% by mass, and even more preferably 0.02% by mass to 2.0% by mass, relative to the total solid content of the photosensitive composition. Furthermore, when the photosensitive composition according to the present disclosure contains a polymerization inhibitor, the content of the polymerization inhibitor in the photosensitive composition is preferably 0.005% by mass to 5.0% by mass, more preferably 0.01% by mass to 3.0% by mass, and even more preferably 0.01% by mass to 1.0% by mass, relative to the total mass of polymerizable monomers.
[0328] <Hydrogen Donor Compound> The photosensitive composition according to the present disclosure may contain a hydrogen donor compound. The hydrogen donor compound has the effect of further improving the sensitivity of the photopolymerization initiator to actinic rays and suppressing the polymerization inhibition of the polymerizable compound caused by oxygen.
[0329] Examples of hydrogen donor compounds include amines and amino acid compounds.
[0330] Examples of amines include compounds described in M. R. Sander et al., "Journal of Polymer Society," Vol. 10, p. 3173 (1972), JP-B No. 44-020189, JP-A No. 51-082102, JP-A No. 52-134692, JP-A No. 59-138205, JP-A No. 60-084305, JP-A No. 62-018537, JP-A No. 64-033104, and Research Disclosure No. 33825. More specifically, examples of the amines include 4,4'-bis(diethylamino)benzophenone, tris(4-dimethylaminophenyl)methane (also known as leuco crystal violet), triethanolamine, p-dimethylaminobenzoic acid ethyl ester, p-formyldimethylaniline, and p-methylthiodimethylaniline. From the viewpoint of achieving superior effects of the present disclosure, the amine is preferably at least one selected from 4,4'-bis(diethylamino)benzophenone and tris(4-dimethylaminophenyl)methane.
[0331] Examples of the amino acid compound include N-phenylglycine, N-methyl-N-phenylglycine, and N-ethyl-N-phenylglycine. Among these, N-phenylglycine is preferred as the amino acid compound from the viewpoint of achieving superior effects of the present disclosure.
[0332] Further, examples of the hydrogen donor compound include organometallic compounds (e.g., tributyltin acetate) described in JP-B-48-042965, hydrogen donors described in JP-B-55-034414, and sulfur compounds (e.g., trithiane) described in JP-A-6-308727.
[0333] When the photosensitive composition according to the present disclosure contains a hydrogen donor compound, it may contain one type of hydrogen donor compound alone, or may contain two or more types of hydrogen donor compounds.
[0334] When the photosensitive composition according to the present disclosure contains a hydrogen donor compound, the content of the hydrogen donor compound in the photosensitive composition is preferably 0.01% by mass to 10.0% by mass, more preferably 0.01% by mass to 8.0% by mass, and even more preferably 0.03% by mass to 5.0% by mass, relative to the total solid content of the photosensitive composition, from the viewpoint of improving the curing rate through a balance between the polymerization propagation rate and chain transfer.
[0335] <Solvent> The photosensitive composition according to the present disclosure may contain a solvent. The solvent may be water or an organic solvent, but an organic solvent is preferred. Examples of organic solvents include methyl ethyl ketone, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate (also known as 1-methoxy-2-propyl acetate), diethylene glycol ethyl methyl ether, cyclohexanone, methyl isobutyl ketone, ethyl lactate, methyl lactate, caprolactam, n-propanol, and 2-propanol.
[0336] The solvent may be an organic solvent having a boiling point of 180° C. to 250° C. (a so-called high-boiling solvent).
[0337] When the photosensitive composition according to the present disclosure contains a solvent, it may contain one type of solvent alone or two or more types of solvents.
[0338] When the photosensitive composition according to the present disclosure contains a solvent, the content of the solvent in the photosensitive composition is preferably 20% by mass to 95% by mass, more preferably 40% by mass to 95% by mass, and even more preferably 60% by mass to 95% by mass, relative to the total mass of the photosensitive composition.
[0339] <Other Additives> The photosensitive composition according to the present disclosure may contain components (also referred to as "other additives") other than the components described above, as necessary, to the extent that the effects of the present disclosure are not impaired. Examples of other additives include colorants (e.g., pigments and dyes), antioxidants, and particles (e.g., metal oxide particles). Other additives also include the other additives described in paragraphs
[0058] to
[0071] of JP 2000-310706 A.
[0340] -Colorant- The photosensitive composition according to the present disclosure may contain a colorant (e.g., a pigment or a dye), but preferably does not substantially contain a colorant, for example, from the viewpoint of transparency. When the photosensitive composition according to the present disclosure contains a colorant, the content of the colorant in the photosensitive composition is preferably less than 1 mass %, and more preferably less than 0.1 mass %, relative to the total solid content of the photosensitive composition.
[0341] -Antioxidant- The photosensitive composition according to the present disclosure may contain an antioxidant. Examples of antioxidants include 3-pyrazolidones such as 1-phenyl-3-pyrazolidone (also known as phenidone), 1-phenyl-4,4-dimethyl-3-pyrazolidone, and 1-phenyl-4-methyl-4-hydroxymethyl-3-pyrazolidone; polyhydroxybenzenes such as hydroquinone, catechol, pyrogallol, methylhydroquinone, and chlorohydroquinone; para-methylaminophenol, para-aminophenol, para-hydroxyphenylglycine, and para-phenylenediamine. As the antioxidant, from the viewpoint of achieving superior effects of the present disclosure, 3-pyrazolidones are preferred, and 1-phenyl-3-pyrazolidone is more preferred.
[0342] When the photosensitive composition according to the present disclosure contains an antioxidant, the content of the antioxidant in the photosensitive composition is preferably 0.001% by mass or more, more preferably 0.005% by mass or more, and even more preferably 0.01% by mass or more, relative to the total solid content of the photosensitive composition. The upper limit is preferably, for example, 1% by mass or less.
[0343] -Particles- The photosensitive composition according to the present disclosure may contain particles. Metal oxide particles are preferred as the particles. Metals in metal oxide particles include semimetals such as B, Si, Ge, As, Sb, and Te. The average primary particle diameter of the particles is preferably 1 nm to 200 nm, and more preferably 3 nm to 80 nm, from the viewpoint of the transparency of the cured film. The average primary particle diameter of the particles is calculated by measuring the particle diameters of 200 random particles using an electron microscope and arithmetically averaging the measurement results. When the shape of the particles is not spherical, the particle diameter is determined as the longest side.
[0344] When the photosensitive composition according to the present disclosure contains particles, it may contain one type of particles or two or more types of particles differing in metal type, size, etc.
[0345] The photosensitive composition according to the present disclosure does not contain particles, or if the photosensitive composition according to the present disclosure contains particles, the particle content is preferably more than 0% by mass and not more than 35% by mass, relative to the total solid content of the photosensitive composition; more preferably, the photosensitive composition does not contain particles, or the particle content is more than 0% by mass and not more than 10% by mass, relative to the total solid content of the photosensitive composition; even more preferably, the photosensitive composition does not contain particles, or the particle content is more than 0% by mass and not more than 5% by mass, relative to the total solid content of the photosensitive composition; even more preferably, the photosensitive composition does not contain particles, or the particle content is more than 0% by mass and not more than 1% by mass, relative to the total solid content of the photosensitive composition; and particularly preferably, the photosensitive composition does not contain particles.
[0346] <<Absorbance of Film>> When a film having a thickness of 1 μm is formed using the photosensitive composition according to the present disclosure, the absorbance of the film at a wavelength of 365 nm (also referred to as "absorbance A1") is preferably 0.1 or less, more preferably 0.08 or less, even more preferably 0.06 or less, and particularly preferably 0.04 or less, from the viewpoint of patterning properties. The lower limit of the absorbance A1 is not particularly limited, and examples thereof include 0.001 or more. An absorbance A1 of 0.1 or less means that a film in a state in which the compound represented by formula (1) has not been colored black by thermal stimulation has excellent transmittance to light having a wavelength of 365 nm. When the absorbance A1 is 0.1 or less, incident light gradually attenuates during exposure in the thickness direction of a film (i.e., a photosensitive composition layer) formed using the photosensitive composition. For example, in the case of a negative type, a phenomenon such as insufficient polymerization and curing is unlikely to occur, and a pattern with a good shape and a high aspect ratio tends to be easily obtained.
[0347] When the photosensitive composition according to the present disclosure is used to cause the compound represented by formula (1) to develop a black color by thermal stimulation to form a black film having a thickness of 1 μm, the absorbance of the film at a wavelength of 365 nm (also referred to as "absorbance A2") is preferably 0.14 or more, more preferably 0.16 or more, even more preferably 0.18 or more, and particularly preferably 0.20 or more. The upper limit of absorbance A2 is not particularly limited, and may be, for example, 4.0 or less.
[0348] The ratio of absorbance A2 to absorbance A1 (absorbance A2 / absorbance A1) is preferably 5.0 or more, and more preferably 7.0 or more.
[0349] When the photosensitive composition according to the present disclosure is used to form a black film having a thickness of 1 μm by causing the compound represented by Formula (1) to develop a black color upon thermal stimulation, the average absorbance (also referred to as "average absorbance B") of the film at wavelengths of 400 nm to 700 nm is preferably 0.14 or more, more preferably 0.16 or more, even more preferably 0.18 or more, and particularly preferably 0.20 or more. The upper limit of the average absorbance B is not particularly limited, and examples include 4.0 or less. The fact that both the absorbance A2 and the average absorbance B are 0.14 or more means that the film in a state in which the compound represented by Formula (1) has developed a black color upon thermal stimulation has excellent light-blocking properties against light with wavelengths from the ultraviolet region to the visible region.
[0350] In the present disclosure, "absorbance" refers to a value measured using a spectrophotometer. For example, an ultraviolet-visible spectrophotometer (model number: UV-1800) manufactured by Shimadzu Corporation can be used as the spectrophotometer. However, the spectrophotometer is not limited to this.
[0351] A preferred embodiment of the photosensitive composition according to the present disclosure comprises a compound represented by formula (1), a specific dispersant, an alkali-soluble resin, a photopolymerizable monomer, and a photopolymerization initiator, and has an absorbance A1 of 0.1 or less, an absorbance A2 of 0.14 or more, and an average absorbance B of 0.14 or more, and a preferred embodiment comprises a compound represented by formula (1), a specific dispersant, an alkali-soluble resin, a photopolymerizable monomer, and a photopolymerization initiator, and has an absorbance A1 of 0.08 or less, an absorbance A2 of 0.16 or more, and an average absorbance B of 0.16 or more. An embodiment comprising a compound represented by formula (1), a specific dispersant, an alkali-soluble resin, a photopolymerizable monomer, and a photopolymerization initiator, in which the absorbance A1 is 0.06 or less, the absorbance A2 is 0.18 or more, and the average absorbance B is 0.18 or more, is even more preferred, and an embodiment comprising a compound represented by formula (1), a specific dispersant, an alkali-soluble resin, a photopolymerizable monomer, and a photopolymerization initiator, in which the absorbance A1 is 0.04 or less, the absorbance A2 is 0.20 or more, and the average absorbance B is 0.20 or more is particularly preferred.
[0352] <<Viscosity of Photosensitive Composition>> The viscosity of the photosensitive composition according to the present disclosure at 25°C is, for example, preferably 1 mPa·s to 50 mPa·s, more preferably 2 mPa·s to 40 mPa·s, and even more preferably 3 mPa·s to 30 mPa·s, from the viewpoint of coatability. The viscosity of the photosensitive composition according to the present disclosure is measured using a viscometer. As the viscometer, for example, a viscometer manufactured by Toki Sangyo Co., Ltd. (product name: VISCOMETER TV-22) can be suitably used. However, the viscometer is not limited to the above-mentioned viscometer.
[0353] <<Surface Tension of Photosensitive Composition>> The surface tension of the photosensitive composition according to the present disclosure at 25°C is, for example, preferably 5 mN / m to 100 mN / m, more preferably 10 mN / m to 80 mN / m, and even more preferably 15 mN / m to 40 mN / m, from the viewpoint of coatability. The surface tension of the photosensitive composition according to the present disclosure is measured using a surface tensiometer. As the surface tensiometer, for example, a surface tensiometer manufactured by Kyowa Interface Science Co., Ltd. (product name: Automatic Surface Tensiometer CBVP-Z) can be suitably used. However, the surface tensiometer is not limited to the above-mentioned surface tensiometer.
[0354] <<Uses of Photosensitive Composition>> The photosensitive composition according to the present disclosure can be used in a variety of applications. The photosensitive composition according to the present disclosure can form a black pattern having a high aspect ratio and excellent light resistance, and therefore can be used in applications such as a black matrix (so-called black partition wall).
[0355] [Method for Producing Photosensitive Composition] The method for producing the photosensitive composition according to the present disclosure is not particularly limited. The photosensitive composition according to the present disclosure can be suitably produced, for example, by the following method. The method for producing the photosensitive composition according to the present disclosure includes a step of preparing a dispersion containing a compound represented by formula (1), a dispersant having an amine value of 70 mgKOH / g or less (i.e., a specific dispersant), and a solvent (hereinafter also referred to as a "dispersion preparation step"), and a step of mixing the dispersion with an alkali-soluble resin, a polymerizable monomer, and a photopolymerization initiator (hereinafter also referred to as a "mixing step"). In the method for producing the photosensitive composition according to the present disclosure, the compound represented by formula (1), the specific dispersant, the alkali-soluble resin, the polymerizable monomer, the photopolymerization initiator, and the solvent are synonymous with the compound represented by formula (1), the specific dispersant, the alkali-soluble resin, the polymerizable monomer, the photopolymerization initiator, and the solvent in the photosensitive composition according to the present disclosure described above, and preferred embodiments are also the same.
[0356] <Dispersion preparation step> The dispersion preparation step is a step of preparing a dispersion containing a compound represented by formula (1), a specific dispersant, and a solvent. In the dispersion preparation step, a dispersant having an amine value of 70 mgKOH / g or less (i.e., a specific dispersant) is used as the dispersant for the compound represented by formula (1) to prepare the dispersion. Therefore, the compound represented by formula (1) is unlikely to develop an unintended color before developing a color due to a thermal stimulus.
[0357] A known dispersing means can be used to prepare the dispersion. A preferred dispersing means is, for example, a mixer, and a more preferred MSE (Multi-Stacked Elements) mixer. A preferred medium is used for dispersion using a mixer. Zirconia beads are a preferred example of the medium. A specific method for preparing the dispersion includes, for example, adding a medium to the compound represented by formula (1), a specific dispersant, and a solvent, and then performing a dispersion treatment using a mixer. The dispersion can be suitably prepared, for example, by the method described in the Examples below.
[0358] <Mixing Step> The mixing step is a step of mixing the dispersion prepared in the dispersion preparation step described above with an alkali-soluble resin, a polymerizable monomer, and a photopolymerization initiator. The mixing method is not particularly limited, and any known mixing method can be used. The dispersion and the alkali-soluble resin, etc. may be mixed together, but it is preferable to add the alkali-soluble resin, etc. to the dispersion while stirring it, as this makes it easier to maintain the dispersed state of the compound represented by formula (1) better.
[0359] The mixing step is preferably a step of mixing the dispersion prepared in the dispersion preparation step with a solution containing an alkali-soluble resin, a polymerizable monomer, a photopolymerization initiator, and a solvent. By mixing a previously prepared dispersion with a solution containing an alkali-soluble resin, etc., this step tends to maintain the dispersion state of the compound represented by formula (1) in a good condition even after mixing. In this case, the solvent contained in the dispersion and the solvent contained in the solution may be the same or different, but are preferably the same.
[0360] [Transfer film] The transfer film according to the present disclosure has a temporary support and a photosensitive composition layer containing the photosensitive composition according to the present disclosure described above. The transfer film according to the present disclosure may have a composition layer other than the photosensitive composition layer (so-called other composition layer). The transfer film according to the present disclosure may have, for example, a configuration having a protective film on the photosensitive composition layer or the other composition layer. The photosensitive composition layer, the other composition layer, and the protective film may each be a single layer, or may be a multi-layer consisting of two or more layers. The transfer film according to the present disclosure preferably has a configuration of temporary support / photosensitive composition layer / protective film.
[0361] In the transfer film according to the present disclosure, when the transfer film further includes another composition layer on the side opposite to the temporary support side of the photosensitive composition layer, the total thickness (total film thickness) of the other composition layers disposed on the side opposite to the temporary support side of the photosensitive composition layer is preferably 0.1% to 30%, and more preferably 0.1% to 20%, of the thickness (film thickness) of the photosensitive composition layer.
[0362] The maximum waviness width of the transfer film according to the present disclosure is preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 60 μm or less, from the viewpoint of preventing the generation of bubbles in the lamination process described below. The lower limit of the maximum waviness width is 0 μm or more, preferably 0.1 μm or more, and more preferably 1 μm or more. The maximum waviness width of the transfer film is a value measured by the following procedure. First, the transfer film is cut in a direction perpendicular to the main surface to a size of 20 cm long x 20 cm wide to prepare a test sample. If the transfer film has a protective film, the protective film is peeled off. Next, the test sample is placed on a flat and horizontal stage with the surface of the temporary support facing the stage. After leaving the test sample to stand, the surface of the test sample is scanned with a laser microscope (for example, VK-9700SP manufactured by Keyence Corporation) over a 10 cm square area in the center of the test sample to obtain a three-dimensional surface image, and the minimum concave height is subtracted from the maximum convex height observed in the obtained three-dimensional surface image. The above operation is performed on 10 test samples, and the arithmetic average value is taken as the "maximum waviness width of the transfer film."
[0363] The configuration of the transfer film according to the present disclosure will be described in detail below.
[0364] <Temporary Support> The transfer film according to the present disclosure has a temporary support. The temporary support is a member that supports the photosensitive composition layer and is ultimately removed by a peeling treatment.
[0365] The temporary support may have a single-layer structure or a multi-layer structure.
[0366] The temporary support is preferably a film, more preferably a resin film. The temporary support is preferably a film that is flexible and does not significantly deform, shrink, or stretch under pressure, or under pressure and heat. Examples of such films include polyethylene terephthalate films (e.g., biaxially oriented polyethylene terephthalate films), polymethyl methacrylate films, cellulose triacetate films, polystyrene films, polyimide films, and polycarbonate films. The temporary support is preferably a polyethylene terephthalate film. It is preferable that the film used as the temporary support is free of deformations such as wrinkles, scratches, etc.
[0367] From the viewpoint of enabling pattern exposure through the temporary support, the temporary support is preferably highly transparent, and the transmittance at wavelengths of 313 nm, 365 nm, 405 nm, and 436 nm is preferably 60% or more, more preferably 70% or more, even more preferably 80% or more, and particularly preferably 90% or more. Preferred values of the transmittance include 87%, 92%, and 98%, etc. The transmittance is calculated as the proportion of light emitted from the temporary support to the amount of light incident at each wavelength (= amount of emitted light / amount of incident light × 100; %).
[0368] From the viewpoint of pattern formability during pattern exposure through the temporary support and transparency of the temporary support, it is preferable that the haze of the temporary support is small. Specifically, the haze value of the temporary support is preferably 2% or less, more preferably 0.5% or less, and even more preferably 0.1% or less. From the viewpoint of pattern formability during pattern exposure through the temporary support and transparency of the temporary support, it is preferable that the number of fine particles, foreign matter and defects contained in the temporary support is small. The total number of fine particles, foreign matter and defects with a diameter of 1 μm or more contained in the temporary support is 50 / 10 mm 2 Preferably, the number is 10 pieces / 10 mm or less. 2 More preferably, it is 3 pieces / 10 mm or less. 2 More preferably, the number is 0 / 10 mm or less. 2It is particularly preferred that:
[0369] In order to improve the adhesion between the temporary support and the photosensitive composition layer, the surface of the temporary support that comes into contact with the photosensitive composition layer may be surface-modified by ultraviolet (UV) irradiation, corona discharge, plasma, or the like.
[0370] When the surface is modified by ultraviolet irradiation, the exposure dose of ultraviolet light is not particularly limited, but is, for example, 10 mJ / cm 2 ~2000mJ / cm 2 and preferably 50 mJ / cm 2 ~1000mJ / cm 2 It is more preferable that:
[0371] Examples of light sources for ultraviolet irradiation include light sources that emit light in the wavelength band of 150 nm to 450 nm, such as low-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, carbon arc lamps, metal halide lamps, xenon lamps, chemical lamps, electrodeless discharge lamps, and light-emitting diodes (LEDs). The lamp output and illuminance are not particularly limited and can be set appropriately depending on, for example, the desired exposure amount.
[0372] In order to provide handleability, a layer containing fine particles (also referred to as a "lubricant layer") may be provided on the surface of the temporary support. The lubricant layer may be provided on one side or both sides of the temporary support. The diameter of the particles contained in the lubricant layer is not particularly limited, but is preferably, for example, 0.05 μm to 0.8 μm. The film thickness of the lubricant layer is not particularly limited, but is preferably, for example, 0.05 μm to 1.0 μm.
[0373] The thickness of the temporary support is not particularly limited, but is preferably 5 μm to 200 μm, and from the viewpoints of handleability and versatility, is more preferably 5 μm to 150 μm, even more preferably 5 μm to 50 μm, and particularly preferably 5 μm to 25 μm. The thickness of the temporary support is calculated as the average value of any five points measured by cross-sectional observation using a scanning electron microscope (SEM).
[0374] Commercially available products can be used as the temporary support. Examples of commercially available products of the temporary support include Lumirror (registered trademark) 16KS40, Lumirror (registered trademark) 16FB40, Lumirror (registered trademark) #38-U48, Lumirror (registered trademark) #75-U34, and Lumirror (registered trademark) #25T60 (all manufactured by Toray Industries, Inc.), and Cosmoshine (registered trademark) A4100, Cosmoshine (registered trademark) A4160, Cosmoshine (registered trademark) A4300, Cosmoshine (registered trademark) A4360, and Cosmoshine (registered trademark) A8300 (all manufactured by Toyobo Co., Ltd.).
[0375] The temporary support may be a recycled product. Examples of recycled products include films made from chips obtained by cleaning used films, etc. Specific examples of recycled products include the Ecouse series manufactured by Toray Industries, Inc.
[0376] Examples of the temporary support include a biaxially oriented polyethylene terephthalate film having a thickness of 16 μm, a biaxially oriented polyethylene terephthalate film having a thickness of 12 μm, and a biaxially oriented polyethylene terephthalate film having a thickness of 9 μm.
[0377] Preferred forms of the temporary support are described, for example, in paragraphs
[0017] to
[0018] of JP 2014-085643 A, paragraphs
[0019] to
[0026] of JP 2016-027363 A, paragraphs
[0041] to
[0057] of WO 2012 / 081680 A, and paragraphs
[0029] to
[0040] of WO 2018 / 179370 A, the contents of which are incorporated herein by reference.
[0378] <Photosensitive composition layer> The transfer film according to the present disclosure has a photosensitive composition layer containing the photosensitive composition according to the present disclosure. With the transfer film according to the present disclosure, a pattern can be formed on the transfer target by transferring the photosensitive composition layer onto the transfer target, followed by exposure and development. The photosensitive composition layer may be any layer containing the photosensitive composition according to the present disclosure, but is preferably a layer made of the photosensitive composition according to the present disclosure or a layer made of the solid content of the photosensitive composition according to the present disclosure.
[0379] The photosensitive composition layer may be a positive photosensitive composition layer or a negative photosensitive composition layer, but is preferably a negative photosensitive composition layer. A negative photosensitive composition layer is a photosensitive composition layer in which the solubility of the exposed portion in a developer decreases upon exposure. When the photosensitive composition layer is a negative photosensitive composition layer, the formed pattern corresponds to a cured layer.
[0380] The photosensitive composition layer may contain a predetermined amount of impurities. Specific examples of impurities include sodium, potassium, magnesium, calcium, iron, manganese, copper, aluminum, titanium, chromium, cobalt, nickel, zinc, tin, halogens, and ions thereof. Among these, halide ions (e.g., chloride ions, bromide ions, and iodide ions), sodium ions, and potassium ions are easily mixed in as impurities, so the following contents are preferred.
[0381] The content of impurities in the photosensitive composition layer is preferably 80 ppm or less, more preferably 10 ppm or less, and even more preferably 2 ppm or less, by mass. The content of impurities in the photosensitive composition layer may be 1 ppb or more, or even 0.1 ppm or more, by mass. A specific example of the content of impurities in the photosensitive composition layer is an embodiment in which all of the above impurities are 0.6 ppm by mass.
[0382] Methods for adjusting the impurity content in the photosensitive composition layer to the above range include, for example, selecting raw materials for the photosensitive composition that have a low impurity content, preventing impurities from being mixed in when the photosensitive composition layer is formed, and removing impurities by washing the photosensitive composition layer. By such methods, the impurity content in the photosensitive composition layer can be adjusted to the above range.
[0383] Impurities can be quantitatively determined by known methods such as ICP (Inductively Coupled Plasma) emission spectroscopy, atomic absorption spectroscopy, and ion chromatography.
[0384] The photosensitive composition layer may contain residual monomers of each structural unit of the alkali-soluble resin described above (hereinafter also simply referred to as "residual monomers"). From the viewpoints of patterning ability and reliability, the content of residual monomers in the photosensitive composition layer is preferably 5,000 ppm by mass or less, more preferably 2,000 ppm by mass or less, and even more preferably 500 ppm by mass or less, relative to the total mass of the alkali-soluble resin. The lower limit is not particularly limited, but may be, for example, 1 ppm by mass or more, or 10 ppm by mass or more.
[0385] From the viewpoints of patterning ability and reliability, the content of residual monomers in the photosensitive composition layer is preferably 3,000 ppm by mass or less, more preferably 600 ppm by mass or less, and even more preferably 100 ppm by mass or less, relative to the total solid content of the photosensitive composition. The lower limit is not particularly limited, but may be, for example, 0.1 ppm by mass or more, or 1 ppm by mass or more.
[0386] The amount of residual monomers in the synthesis of an alkali-soluble resin by a polymer reaction is also preferably within the above range. For example, when the alkali-soluble resin is synthesized by reacting glycidyl acrylate with a carboxylic acid side chain, the content of glycidyl acrylate is preferably within the above range.
[0387] The amount of residual monomer in the photosensitive composition layer can be measured by a known method such as liquid chromatography or gas chromatography.
[0388] The content of compounds such as benzene, formaldehyde, trichloroethylene, 1,3-butadiene, carbon tetrachloride, chloroform, N,N-dimethylformamide, N,N-dimethylacetamide, and hexane in the photosensitive composition layer is preferably low. The content of these compounds in the photosensitive composition layer is preferably 100 ppm or less, more preferably 20 ppm or less, and even more preferably 4 ppm or less, by mass. The lower limit can be 10 ppb or more, and can be 100 ppb or more, by mass. The content of these compounds can be reduced, for example, by selecting raw materials for the photosensitive composition that contain low amounts of these compounds and by preventing the inclusion of these compounds during the formation of the photosensitive composition layer. The content of these compounds can be quantified by known measurement methods.
[0389] The water content in the photosensitive composition layer is preferably 0.01% by mass to 1.0% by mass, and more preferably 0.05% by mass to 0.5% by mass, from the viewpoint of improving reliability and lamination properties.
[0390] <<Thickness of Photosensitive Composition Layer>> The thickness of the photosensitive composition layer (also referred to as "film thickness") is not particularly limited. The film thickness of the photosensitive composition layer is, for example, preferably 5 μm or more, and more preferably 10 μm or more, from the viewpoint of further suppressing color mixing of light between adjacent pixels when used as a partition wall of a micro LED display. From the viewpoint of further suppressing color mixing when a black pattern is formed, the film thickness of the photosensitive composition layer is preferably 10 μm or more, more preferably 20 μm or more, even more preferably 30 μm or more, and particularly preferably 50 μm or more. Furthermore, from the viewpoint of handleability, the film thickness of the photosensitive composition layer is preferably 100 μm or less, more preferably 80 μm or less, even more preferably 20 μm or less, and particularly preferably 15 μm or less.
[0391] The film thickness of the photosensitive composition layer is calculated as the average value of measurements taken at any five points by cross-sectional observation using a scanning electron microscope (SEM).
[0392] <<Refractive Index of Photosensitive Composition Layer>> The refractive index of the photosensitive composition layer is not particularly limited, but is preferably 1.41 to 1.59, and more preferably 1.47 to 1.56. The refractive index of the photosensitive composition layer is a value measured at a wavelength of 550 nm using an ellipsometer in an environment with an ambient temperature of 25°C.
[0393] <<Color of Photosensitive Composition Layer>> The photosensitive composition layer is preferably achromatic. Specifically, the total reflection (incident angle: 8°, light source: D-65 (2° visual field)) is preferably L*, a*, b* in the CIE 1976 (L*, a*, b*) color space. * The value is preferably 10 to 90, and a * The value is preferably −1.0 to 1.0, and b * The value is preferably between −1.0 and 1.0.
[0394] <<Dissolution Rate of Photosensitive Composition Layer>> The dissolution rate of the photosensitive composition layer in a 1.0 mass % aqueous sodium carbonate solution is preferably 0.01 μm / sec or more, more preferably 0.10 μm / sec or more, and even more preferably 0.20 μm / sec or more, from the viewpoint of suppressing residues during development. Furthermore, the dissolution rate of the photosensitive composition layer in a 1.0 mass % aqueous sodium carbonate solution is preferably 5.0 μm / sec or less, more preferably 4.0 μm / sec or less, and even more preferably 3.0 μm / sec or less, from the viewpoint of the edge shape of the pattern. Specific preferred values include 1.8 μm / sec, 1.0 μm / sec, and 0.7 μm / sec.
[0395] The dissolution rate per unit time of a photosensitive composition layer in a 1.0 mass % sodium carbonate aqueous solution is measured as follows. A photosensitive composition layer (with a film thickness in the range of 1.0 μm to 10 μm) formed on a glass substrate and from which the solvent has been thoroughly removed is subjected to shower development using a 1.0 mass % sodium carbonate aqueous solution at a liquid temperature of 25°C until the photosensitive composition layer is completely dissolved (however, this is limited to a maximum of 2 minutes). The film thickness of the photosensitive composition layer is determined by dividing it by the time required for the photosensitive composition layer to completely dissolve. If the photosensitive composition layer is not completely dissolved within 2 minutes, the dissolution rate is calculated in the same manner from the amount of film thickness change up to that point. A shower nozzle (model number: 1 / 4MINJJX030PP) manufactured by Ikeuchi Co., Ltd. is used for development, and the shower spray pressure is 0.08 MPa. Under the above conditions, the shower flow rate per unit time is 1,800 mL / min.
[0396] <<Dissolution Rate of Cured Film of Photosensitive Composition Layer>> The dissolution rate of a cured film of the photosensitive composition layer (having a film thickness in the range of 1.0 μm to 10 μm) in a 1.0 mass % aqueous sodium carbonate solution is preferably 3.0 μm / sec or less, more preferably 2.0 μm / sec or less, even more preferably 1.0 μm / sec or less, and particularly preferably 0.2 μm / sec or less. The cured film of the photosensitive composition layer is formed by exposing the photosensitive composition layer to i-rays (wavelength 365 nm) at an exposure dose of 300 mJ / cm. 2 Specific preferred values include 0.8 μm / sec, 0.2 μm / sec, and 0.001 μm / sec.
[0397] The dissolution rate of the cured film of the photosensitive composition layer (within the film thickness range of 1.0 μm to 10 μm) in a 1.0 mass % aqueous sodium carbonate solution is measured in the same manner as the above-described dissolution rate per unit time of the photosensitive composition layer in a 1.0 mass % aqueous sodium carbonate solution.
[0398] <<Swelling Ratio of Photosensitive Composition Layer>> From the viewpoint of improving pattern formability, the swelling ratio of the photosensitive composition layer after exposure to a 1.0 mass % aqueous sodium carbonate solution is preferably 100% or less, more preferably 50% or less, and even more preferably 30% or less. The swelling ratio of the photosensitive composition layer after exposure to a 1.0 mass % aqueous sodium carbonate solution is measured as follows: A photosensitive composition layer (thickness in the range of 1.0 μm to 10 μm) formed on a glass substrate and from which the solvent has been thoroughly removed is exposed to i-line (wavelength 365 nm) using an ultra-high pressure mercury lamp at an exposure dose of 500 mJ / cm. 2 The glass substrate is immersed in a 1.0 mass % sodium carbonate aqueous solution at a liquid temperature of 25°C, and the film thickness is measured after 30 seconds. The percentage increase in film thickness after immersion relative to the film thickness before immersion is then calculated. Specific preferred values include 4%, 13%, 25%, etc.
[0399] <<Foreign matter in the photosensitive composition layer>> The number of foreign matter with a diameter of 1.0 μm or more in the photosensitive composition layer is set to 10 particles / mm from the viewpoint of pattern formability. 2 It is preferable that the number of particles is 5 or less per mm. 2 The number of foreign particles in the photosensitive composition layer is measured as follows: Five randomly selected regions (1 mm x 1 mm) on the surface of the photosensitive composition layer are visually observed using an optical microscope from the normal direction of the surface of the photosensitive composition layer. The number of foreign particles having a diameter of 1.0 μm or more in each region is measured, and the arithmetic average of these is calculated as the number of foreign particles. A specific preferred numerical value is 0 particles / mm 2 , 1 piece / mm 2 , 4 pieces / mm 2 , 8 pieces / mm 2 etc.
[0400] <<Haze of dissolved material in photosensitive composition layer>> A 1.0 mass % sodium carbonate aqueous solution (1.0 L) at a liquid temperature of 30°C was dissolved in 1.0 cm 3The haze of the solution obtained by dissolving the photosensitive composition layer is preferably 60% or less, more preferably 30% or less, even more preferably 10% or less, and particularly preferably 1% or less, from the viewpoint of preventing the generation of aggregates during development.
[0401] The haze is measured as follows: First, a 1.0 mass % aqueous sodium carbonate solution is prepared, and the liquid temperature is adjusted to 30° C. Next, 1.0 cm 3 is added to 1.0 L of the 1.0 mass % aqueous sodium carbonate solution at a liquid temperature of 30° C. 3 The photosensitive composition layer is placed in the solution. The mixture is stirred at 30°C for 4 hours, taking care not to introduce air bubbles. After stirring, the haze of the solution in which the photosensitive composition layer has been dissolved is measured. The haze is measured using a haze meter as the measuring device, using a liquid measurement unit and a dedicated liquid measurement cell with an optical path length of 20 mm. A suitable haze meter is, for example, a haze meter (model number: NDH4000) manufactured by Nippon Denshoku Industries Co., Ltd. However, the haze meter is not limited to the above. Specific preferred values include 0.4%, 1.0%, 9%, and 24%.
[0402] <Protective Film> The transfer film according to the present disclosure may have a protective film. Examples of the protective film include resin films having heat resistance and solvent resistance. Examples of the protective film include polyolefin films (e.g., polypropylene films and polyethylene films), polyester films (e.g., polyethylene terephthalate films), polycarbonate films, and polystyrene films. As the protective film, polyolefin films are preferred, polypropylene films or polyethylene films are more preferred, and polyethylene films are even more preferred. It is also preferable to use a resin film made of the same material as the temporary support described above as the protective film.
[0403] The thickness of the protective film is preferably 1 μm to 100 μm, more preferably 5 μm to 50 μm, even more preferably 10 μm to 40 μm, and particularly preferably 15 μm to 30 μm. The thickness of the protective film is preferably 1 μm or more from the viewpoint of excellent mechanical strength, and is preferably 100 μm or less from the viewpoint of being relatively inexpensive.
[0404] The number of fisheyes with a diameter of 80 μm or more contained in the protective film is 5 per 1 m. 2 The following is preferable: "Fisheyes" are foreign matter, undissolved matter, oxidized and deteriorated matter, etc., of the material that is introduced into the film when the material is thermally melted and then kneaded, extruded, biaxially stretched, cast, or other methods are used to produce the film.
[0405] The number of particles with a diameter of 3 μm or more contained in the protective film is 30 / mm 2 It is preferable that the number of particles is 10 or less per mm. 2 More preferably, the number is 5 or less per mm 2 It is more preferable that the following is satisfied: This makes it possible to suppress defects caused by unevenness due to particles contained in the protective film being transferred to the photosensitive composition layer.
[0406] From the viewpoint of providing windability, the arithmetic mean roughness Ra of the surface of the protective film opposite to the surface in contact with the photosensitive composition layer is preferably 0.01 μm or more, more preferably 0.02 μm or more, and even more preferably 0.03 μm or more, while the arithmetic mean roughness Ra of the surface of the protective film opposite to the surface in contact with the photosensitive composition layer is preferably less than 0.50 μm, more preferably 0.40 μm or less, and even more preferably 0.30 μm or less.
[0407] From the viewpoint of suppressing defects during transfer, the arithmetic surface roughness Ra of the surface of the protective film in contact with the photosensitive composition layer is preferably 0.01 μm or more, more preferably 0.02 μm or more, and even more preferably 0.03 μm or more, while the arithmetic surface roughness Ra of the surface of the protective film in contact with the photosensitive composition layer is preferably less than 0.50 μm, more preferably 0.40 μm or less, and even more preferably 0.30 μm or less.
[0408] The protective film may be a recycled product. Examples of recycled products include films made from chips obtained by cleaning used films, etc. Specific examples of recycled products include the Ecouse series manufactured by Toray Industries, Inc.
[0409] <<Relationship Between Temporary Support, Photosensitive Composition Layer, and Protective Film>> In the transfer film according to the present disclosure, it is preferred that the cured film obtained by curing the photosensitive composition layer has a breaking elongation at 120°C of 15% or more, the arithmetic mean roughness Ra of the surface of the temporary support facing the photosensitive composition layer is 50 nm or less, and the arithmetic mean roughness Ra of the surface of the protective film facing the photosensitive composition layer is 150 nm or less.
[0410] The transfer film according to the present disclosure preferably satisfies the following formula (T1): X × Y < 1500 ... formula (T1) In formula (T1), X represents the breaking elongation (%) at 120°C of the cured film obtained by curing the photosensitive composition layer, and Y represents the arithmetic mean roughness Ra (nm) of the surface of the temporary support on the photosensitive composition layer side. X × Y is more preferably 750 or less. Specific values of X include 18%, 25%, 30%, and 35%, etc. Specific values of Y include 4 nm, 8 nm, 15 nm, and 30 nm, etc. Specific values of X × Y include 150, 200, 300, 360, and 900, etc.
[0411] In the transfer film according to the present disclosure, it is preferable that the breaking elongation at 120°C of the cured film obtained by curing the photosensitive composition layer is at least twice as large as the breaking elongation at 23°C of the cured film obtained by curing the photosensitive composition layer.
[0412] The breaking elongation was measured by exposing a 20 μm thick photosensitive composition layer to an exposure dose of 120 mJ / cm using an ultra-high pressure mercury lamp. 2 After curing by exposure to 400 mJ / cm using a high-pressure mercury lamp, 2 The cured film is then heated at 145° C. for 30 minutes, and the test sample is subjected to a tensile test.
[0413] The transfer film according to the present disclosure preferably satisfies the following formula (T2): Y≦Z formula (T2) In formula (T2), Y represents the value (nm) of the arithmetic mean roughness Ra of the surface of the temporary support facing the photosensitive composition layer, and Z represents the value (nm) of the arithmetic mean roughness Ra of the surface of the protective film facing the photosensitive composition layer.
[0414] <<Uses of Transfer Film>> The transfer film according to the present disclosure can be used for various purposes. For example, the transfer film according to the present disclosure can be used for a black matrix (so-called black partition wall).
[0415] <Method of manufacturing transfer film> The method of manufacturing the transfer film according to the present disclosure is not particularly limited, and a known method can be used. For example, from the viewpoint of excellent productivity, the method of manufacturing the transfer film according to the present disclosure can be a method including a step of applying a photosensitive composition to the surface of a temporary support to form a coating film, and a step of drying the formed coating film to form a photosensitive composition layer.
[0416] Examples of methods for applying the photosensitive composition include printing, spraying, roll coating, bar coating, curtain coating, spin coating, and die coating (i.e., slit coating).
[0417] Examples of drying methods for the coating film include natural drying, heat drying, and reduced pressure drying, and these drying methods can be applied alone or in combination. Heat drying and / or reduced pressure drying are preferred as drying methods for the coating film. In the present disclosure, "drying" means removing at least a portion of the solvent contained in the composition. The drying temperature is preferably 80°C or higher, more preferably 90°C or higher. The upper limit of the drying temperature is preferably 130°C or lower, more preferably 120°C or lower. Drying may be performed by continuously changing the temperature. The drying time is preferably 20 seconds or longer, more preferably 40 seconds or longer, and even more preferably 60 seconds or longer. The upper limit of the drying time is not particularly limited, but is preferably, for example, 600 seconds or shorter, more preferably 300 seconds or shorter.
[0418] When the transfer film according to the present disclosure has a protective film on the side of the photosensitive composition layer opposite the temporary support, for example, the protective film can be pressed onto and bonded to the photosensitive composition layer formed above, thereby producing a transfer film having a configuration of temporary support / photosensitive composition layer / protective film.
[0419] The method for laminating the protective film and the photosensitive composition layer is not particularly limited, and known methods can be used. For example, known laminators such as a vacuum laminator or an auto laminator can be used to laminate the protective film and the photosensitive composition layer. The laminator is preferably equipped with any heatable roller such as a rubber roller and capable of applying pressure and heat.
[0420] The transfer film produced as described above may be wound up to prepare a roll of transfer film and stored. The roll of transfer film can be provided as is for the lamination step with a substrate in a roll-to-roll system.
[0421] [Method for manufacturing laminate] The method for manufacturing a laminate according to the present disclosure is a method for manufacturing a laminate having a black pattern, and includes, in this order, a step of forming a photosensitive composition layer containing the photosensitive composition according to the present disclosure on a substrate (hereinafter also referred to as a "forming step"), a step of patternwise exposing the photosensitive composition layer (hereinafter also referred to as an "exposing step"), and a step of developing the photosensitive composition layer (hereinafter also referred to as a "developing step"), and includes, after the patternwise exposing step, a step of causing the compound represented by formula (1) to develop a black color (hereinafter also referred to as a "coloring step"). The procedures of the above steps will be described in detail below.
[0422] <Forming step> The forming step is a step of forming a photosensitive composition layer containing the photosensitive composition according to the present disclosure on a substrate. The forming step may be a step of forming a photosensitive composition layer containing the photosensitive composition according to the present disclosure on a substrate, and may be, for example, a step of forming a photosensitive composition layer by forming a coating film of the photosensitive composition according to the present disclosure on a substrate and drying the formed coating film, or may be a step of forming a photosensitive composition layer on a substrate by contacting the surface of the photosensitive composition layer of the transfer film according to the present disclosure opposite to the temporary support with the substrate and laminating it (hereinafter also referred to as "lamination step"). However, it is preferably a lamination step.
[0423] In the laminating step, the surface of the photosensitive composition layer of the transfer film according to the present disclosure opposite the temporary support is brought into contact with the substrate and laminated to form a photosensitive composition layer on the substrate. Note that, when the transfer film according to the present disclosure has a protective film on the surface of the photosensitive composition layer opposite the temporary support, the protective film is peeled off before the laminating step is carried out.
[0424] The method for laminating the photosensitive composition layer and the substrate is not particularly limited, and known methods can be used. For example, known laminators such as a vacuum laminator or an auto laminator can be used to laminate the photosensitive composition layer and the substrate. The laminator is preferably equipped with any heatable roller such as a rubber roller and capable of applying pressure and heat. The lamination temperature is preferably, for example, 70°C to 130°C.
[0425] The substrate is preferably a glass substrate or a resin substrate. A transparent substrate is preferred, and a transparent resin substrate is more preferred. The refractive index of the substrate is preferably 1.50 to 1.52. Examples of glass substrates include tempered glass such as Corning Gorilla Glass (registered trademark). The thickness of the glass substrate is preferably 0.01 mm to 1.1 mm, and more preferably 0.1 mm to 0.7 mm. Examples of resin substrates include substrates made of resins such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polycarbonate (PC), triacetyl cellulose (TAC), polyimide (PI), polybenzoxazole (PBO), and cycloolefin polymer (COP). The thickness of the resin substrate is preferably 5 μm to 200 μm, and more preferably 10 μm to 100 μm. As the material of the substrate, for example, the materials described in JP-A Nos. 2010-86684, 2010-152809, and 2010-257492 are preferably used.
[0426] <Exposure Step> The exposure step is a step of patternwise exposing the photosensitive composition layer. "Patternwise exposure" refers to a form of patternwise exposure, that is, exposure in a form in which exposed and non-exposed areas exist. The positional relationship between the exposed and non-exposed areas in the patternwise exposure is not particularly limited and can be adjusted as appropriate. For example, when the photosensitive composition layer is a negative type, the exposed areas in the photosensitive composition layer on the substrate are cured in the patternwise exposure, and ultimately become a cured film. On the other hand, the non-exposed areas in the photosensitive composition layer on the substrate are not cured, and are dissolved and removed by a developer in the development step described below. The non-exposed areas can form openings in the cured film after the development step.
[0427] The light source for the patterned exposure can be appropriately selected and used as long as it can irradiate light in a wavelength range (e.g., 365 nm or 405 nm) that can cure the photosensitive composition layer. In particular, the dominant wavelength of the exposure light for the patterned exposure is preferably 365 nm. The dominant wavelength refers to the wavelength with the highest intensity.
[0428] Examples of light sources include various lasers, light-emitting diodes (LEDs), ultra-high pressure mercury lamps, high pressure mercury lamps, and metal halide lamps. 2 ~200 mJ / cm 2 and preferably 10 mJ / cm 2 ~200 mJ / cm 2 It is more preferable that:
[0429] When a photosensitive composition layer is formed on a substrate using a transfer film, pattern exposure may be performed after peeling off the temporary support, or pattern exposure may be performed via the temporary support before peeling off the temporary support, and then the temporary support may be peeled off. From the viewpoint of preventing contamination of the mask due to contact with the photosensitive composition layer and avoiding the influence of foreign matter attached to the mask on the exposure, it is preferable to perform pattern exposure without peeling off the temporary support. From the viewpoint of suppressing scattering of exposure light by the temporary support and suppressing diffraction of light transmitted through the mask, thereby improving resolution, it is preferable to perform pattern exposure after peeling off the temporary support.
[0430] The pattern exposure may be exposure through a mask, or digital exposure using a laser or the like. Examples of the mask substrate when exposure is performed through a mask include a quartz mask, a soda lime glass mask, and a film mask. Among these, a quartz mask is preferred as the mask substrate because of its excellent dimensional accuracy, and a film mask is preferred because it can be easily made into a large size. A polyester film is preferred as the mask substrate, and a polyethylene terephthalate film is more preferred. A specific example of a film mask substrate is XPR-7S SG (manufactured by Fujifilm Global Graphic Systems Co., Ltd.).
[0431] Preferred embodiments of the light source, exposure dose, and exposure method used for exposure are described, for example, in paragraphs
[0146] to
[0147] of WO 2018 / 155193, the contents of which are incorporated herein by reference.
[0432] Furthermore, when the transfer film according to the present disclosure is used in the exposure process, alignment of the substrate and the mask can be easily performed with high accuracy. The alignment method is not particularly limited, and known methods can be used. One example of an alignment method is to provide alignment marks on the surface of the substrate and the mask in advance, and then adjust the relative positions of the substrate and the mask so that the positions of the alignment marks on the substrate surface and the alignment marks on the mask coincide with each other through camera observation, followed by exposure. When carbon black, which has traditionally been widely used for partition walls, is used as a colorant, it is difficult to observe the alignment marks because carbon black absorbs visible light. On the other hand, when a compound represented by formula (1) is used as in the present disclosure, it is easy to observe the alignment marks.
[0433] <Development Step> The development step is a step of developing the photosensitive composition layer after patternwise exposure. A pattern is formed by developing the photosensitive composition layer after patternwise exposure. The photosensitive composition layer after patternwise exposure can be developed using a developer. The developer is preferably an alkaline aqueous solution. Examples of alkaline compounds that can be contained in the alkaline aqueous solution include sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, and choline (2-hydroxyethyltrimethylammonium hydroxide). The pH of the alkaline aqueous solution at 25°C is preferably 8 to 13, more preferably 9 to 12, and even more preferably 10 to 12. The content of the alkaline compound in the alkaline aqueous solution is preferably 0.1 to 5% by mass, more preferably 0.1 to 3% by mass, relative to the total mass of the alkaline aqueous solution. In the present disclosure, examples of developers that can be suitably used include the developers described in paragraph
[0194] of WO 2015 / 093271.
[0434] Examples of the development method include puddle development, shower development, spin development, dip development, etc. In the present disclosure, examples of the development method that can be suitably used include the development method described in paragraph
[0195] of WO 2015 / 093271.
[0435] The development step may include a step of carrying out the development and a step of heat-treating (also referred to as "post-baking") the pattern obtained by the development. The post-baking temperature is preferably 80°C to 260°C, more preferably 90°C to 160°C. The post-baking time is preferably 1 minute to 180 minutes, more preferably 10 minutes to 60 minutes. Furthermore, exposure may be further carried out after the development step and before the color-developing step. Examples of light sources for this exposure include the same light sources as those described for the pattern exposure. The exposure dose is 100 mJ / cm 2 ~5000mJ / cm 2 and preferably 300 mJ / cm 2 ~2000mJ / cm 2 It is more preferable that:
[0436] <Color Development Step> The production method according to the present disclosure includes a step of causing the compound represented by formula (1) contained in the photosensitive composition layer to develop a black color (i.e., a color development step) after the step of patternwise exposure (i.e., an exposure step). The color development step may be performed after the exposure step, for example, during or after the development step. "After the exposure step" means "after exposure for curing the photosensitive composition layer." In the color development step, for example, the photosensitive composition layer is heated to apply a thermal stimulus to the compound represented by formula (1) contained in the photosensitive composition layer, thereby causing the compound represented by formula (1) to develop a black color. The post-baking step may also serve as the color development step.
[0437] The method for heating the photosensitive composition layer is not particularly limited, and known heating methods can be used. Examples of heating means include an oven, a hot plate, and a heat roll. The heating temperature is not particularly limited as long as it is a temperature at which the compound represented by formula (1) develops a black color, and a heating temperature of 80°C to 260°C is preferred. The heating time is not particularly limited and can be appropriately set depending on the degree of color development. For example, it can be 1 minute to 120 minutes. When the photosensitive composition layer contains a thermoplastic resin, it is preferable to appropriately adjust the heating time, such as shortening it, in consideration of maintaining the pattern shape. A specific example of heating is heating for 3 minutes to 60 minutes in a convection oven set at 150°C to 230°C.
[0438] A preferred method for causing the compound represented by formula (1) to develop a black color is to perform post-baking in the development step, thereby applying a thermal stimulus to the compound represented by formula (1) contained in the photosensitive composition layer and causing the compound represented by formula (1) to develop a black color. In this method, the pattern containing the compound represented by formula (1) obtained by development is heated during post-baking, causing the compound represented by formula (1) to react with oxygen in the air and become an oxidant, thereby causing the compound to develop a black color.
[0439] For example, when forming a negative-pattern black matrix, if the exposed film is black, the exposure light is absorbed, causing the incident light to gradually attenuate in the thickness direction of the photosensitive composition layer used to form the pattern. Due to insufficient polymerization and curing, it is difficult to obtain a pattern with a good shape and a high aspect ratio after development. In contrast, in the production method according to the present disclosure, the photosensitive composition layer is exposed to light before the compound represented by formula (1) develops a black color upon thermal stimulation. The photosensitive composition layer contains the compound represented by formula (1) and a specific dispersant, and the compound represented by formula (1) is unlikely to develop an unintended color before developing a color upon thermal stimulation. Therefore, during pattern exposure, the exposure light is unlikely to be absorbed, and the phenomenon of the incident light gradually attenuating in the thickness direction of the photosensitive composition layer is unlikely to occur. Sufficient polymerization and curing is achieved, making it possible to form a black pattern with a high aspect ratio.
[0440] [Laminate manufactured by the manufacturing method according to the present disclosure] The laminate manufactured by the manufacturing method according to the present disclosure has a black pattern. The black pattern of the laminate manufactured by the manufacturing method according to the present disclosure has a high aspect ratio and excellent light resistance.
[0441] The film thickness of the black pattern in the laminate produced by the production method according to the present disclosure is preferably 5 μm or more, more preferably 10 μm or more. If the film thickness of the black pattern is 5 μm or more, for example, when the black pattern is used as a partition wall, color mixing between pixels tends to be further suppressed. From the viewpoint of further suppressing color mixing, the film thickness of the black pattern is preferably 10 μm or more, more preferably 20 μm or more, even more preferably 30 μm or more, and particularly preferably 50 μm or more. From the viewpoint of handleability, the upper limit is preferably 100 μm or less, more preferably 80 μm or less. In one embodiment, the film thickness of the black pattern may be 5 μm to 100 μm, 5 μm to 80 μm, 5 μm to 50 μm, 5 μm to 20 μm, 5 μm to 15 μm, 10 μm to 100 μm, 20 μm to 100 μm, 30 μm to 80 μm, or 50 μm to 80 μm.
[0442] The absorbance at a wavelength of 365 nm of the black pattern of the laminate produced by the production method according to the present disclosure is preferably 2.0 or more, more preferably 3.0 or more. The upper limit is not particularly limited, and may be, for example, 5.0 or less.
[0443] The black pattern in the laminate produced by the production method according to the present disclosure preferably has an aspect ratio, which is the ratio of the film thickness to the line width of the bottom, of 1 or more, more preferably 5 or more, and even more preferably 10 or more. The upper limit is not particularly limited, and may be, for example, 30 or less.
[0444] In the present disclosure, the aspect ratio, which is the ratio of film thickness to bottom line width, is determined by observing the cross section of the black pattern using a scanning electron microscope (SEM), measuring the film thickness and bottom line width of the black pattern, and then using the following formula: "Aspect ratio" = "Film thickness" / "Bottom line width"
[0445] The black pattern of the laminate produced by the production method according to the present disclosure preferably satisfies the relationship 0.15≦X / Y, more preferably 0.2≦X / Y, and even more preferably 0.3≦X / Y, where X is the average absorbance at wavelengths of 400 nm to 600 nm and Y μm is the film thickness. The upper limit of X / Y is not particularly limited, and may be, for example, 2 or less.
[0446] The present disclosure will be described in more detail below with reference to examples. The materials, amounts used, ratios, processing details, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present disclosure. Therefore, the scope of the present disclosure should not be interpreted as being limited by the examples shown below. Unless otherwise specified, "%" is based on mass. In the following examples, the weight average molecular weight of the resin is the weight average molecular weight determined in terms of polystyrene by gel permeation chromatography (GPC).
[0447] [Synthesis of Binder Polymer P-1] 82.4 g of propylene glycol monomethyl ether (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was placed in a 1000 mL flask and heated to 90° C. under a nitrogen stream. To the heated propylene glycol monomethyl ether, a solution prepared by dissolving 38.4 g of styrene (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.), 30.1 g of dicyclopentanyl methacrylate (trade name: FANCRIL (registered trademark) FA-513M, manufactured by Resonac Corporation), and 34.0 g of methacrylic acid (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) in 20 g of propylene glycol monomethyl ether, and a solution prepared by dissolving 5.4 g of dimethyl 2,2′-azobis(2-methylpropionate) (trade name: V-601, manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) as a polymerization initiator in 43.6 g of propylene glycol monomethyl ether acetate (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) were simultaneously added dropwise over 3 hours. After the dropwise addition was completed, 0.75 g of polymerization initiator (V-601) was added to the solution three times every hour. The solution was then allowed to react for an additional three hours. The resulting solution was then diluted with 58.4 g of propylene glycol monomethyl ether acetate and 11.7 g of propylene glycol monomethyl ether. The diluted solution was then heated to 100°C under an air stream. To the heated solution were then added 0.53 g of tetraethylammonium bromide (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) and 0.26 g of p-methoxyphenol (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.). To the resulting solution, 25.5 g of glycidyl methacrylate (trade name: Blemmer (registered trademark) GH, manufactured by NOF Corporation) was then added dropwise over 20 minutes. The resulting solution was then allowed to react at 100°C for seven hours, yielding 350.6 g of a solution of binder polymer P-1.
[0448] The solids concentration of the resulting solution was 36.3% by mass. The resulting binder polymer P-1 contained the structural units shown in Table 1 below, and had a weight average molecular weight (Mw) of 17,000, a polydispersity (Mw / Mn) of 2.4, and an acid value of 94.5 mgKOH / g.
[0449]
[0450] The weight average molecular weight (Mw) and number average molecular weight (Mn) of binder polymer P-1 were determined by gel permeation chromatography (GPC) in terms of standard polystyrene. The acid value of binder polymer P-1 was measured according to the method described in JIS K0070:1992. The amount of residual monomer measured using gas chromatography (GC) was less than 0.1% by mass of the solid content of binder polymer P-1 for each monomer. The term "solid content" refers to all components of the binder polymer P-1 solution excluding the solvent, and even if the components are in a liquid state, they are included in the solid content.
[0451] In Table 1, structural units other than those having a (meth)acryloyl group are shown by the abbreviation of the monomer that forms each structural unit. Structural units having a (meth)acryloyl group are shown in the form of an addition structure between monomers. For example, MAA-GMA means a structural unit in which glycidyl methacrylate (GMA) is added to a structural unit derived from methacrylic acid (MAA).
[0452] The following abbreviations represent the following monomers: "St": styrene, "MAA": methacrylic acid, "GMA": glycidyl methacrylate, "DCPMA": dicyclopentanyl methacrylate.
[0453] [Synthesis of Colorant Precursor] The following compounds (1) and (2) were synthesized based on the following scheme. Note that N—R in the scheme represents Y in formula (1). 2 Corresponds to.
[0454]
[0455]
[0456] [Synthesis of Compound (1)] A compound corresponding to the black compound in the above scheme [compound (100)] was synthesized using isatin as the starting material, with reference to J. Am. Chem. Soc. 2015, 137, 15947-15956. To a 300 mL three-neck flask, 150 mL of tetrahydrofuran (THF) [stabilizer-containing, Wako First Grade, Fujifilm Wako Pure Chemical Industries, Ltd.] was added, followed by 10.0 g of the synthesized compound (100) and 4.9 g of zinc powder [Wako Special Grade, Fujifilm Wako Pure Chemical Industries, Ltd.]. The three-neck flask was immersed in ice water to maintain the internal temperature below 5°C, and 15 mL of trifluoroacetic acid [Wako Special Grade, Fujifilm Wako Pure Chemical Industries, Ltd.] was added dropwise. After the addition was complete, the external equipment was removed, and the mixture was allowed to react in a water bath for 2 hours, ensuring that the internal temperature did not exceed 40°C. The reaction solution was filtered through Celite, and 10 mL of ultrapure water was added to the filtrate. The mixture was heated to 40°C and THF was distilled off under reduced pressure. The precipitated gray solid was filtered by suction and washed with 300 mL of ultrapure water. The solid was dried for 12 hours using a blower dryer set at 50°C to obtain 4.5 g of compound (1) (yield: 46%).
[0457]
[0458] 1 The structure of the obtained compound (1) was confirmed to be the same as that of the above-mentioned compound (1) by H-NMR. The NMR data of the obtained compound (1) are shown below.
[0459] <NMR data of compound (1)> 1 H-NMR (CDCl3-d) δ = 0.80-1.90 (m, 30H), 3.30-3.70 (m, 4H), 4.20-4.50(s×3, 4H), 6.20-6.50 (m, 2H), 6.80-7.20 (m, 6H), 7.30-7.40 (m, 2H)
[0460] [Synthesis of Compound (2)] In the above scheme, a black compound [compound (101) having the following structure] was synthesized directly from isatin without passing through an isatin derivative. 100 mL of N,N-dimethylformamide (DMF) [Wako Special Grade, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.] was added to a 300 mL three-neck flask, followed by 10.0 g of compound (101) and 1.0 g of Palladium 10% on Carbon [trade name, manufactured by Tokyo Chemical Industry Co., Ltd.]. A balloon filled with nitrogen was attached to the flask, and the flask was degassed and then replaced with nitrogen. The reaction was carried out for 2 hours at room temperature (25°C) under a nitrogen atmosphere. The reaction solution was filtered through Celite, and the Celite was washed with ethyl acetate. The filtrate was placed in an evaporator in a 40°C water bath, and the ethyl acetate was removed, yielding a DMF solution containing the target compound. This DMF solution was purified by silica gel column chromatography, and the fraction containing the target compound was again subjected to evaporation to obtain 10 mg (yield 0.22%) of a gray precipitated compound (2).
[0461]
[0462] 1 The structure of the obtained compound (2) was confirmed to be the same as that of the above-mentioned compound (2) by H-NMR. The NMR data of the obtained compound (2) are shown below.
[0463] <NMR data of compound (2)> 1 H-NMR (DMSO-d 6 ) δ = 4.25-4.40 (m, 2H), 4.75-4.84 (m, 2H),6.47-6.55 (m, 1H), 6.70-7.00 (m, 7H), 7.10-7.32 (m, 2H)
[0464] [Color Evaluation of Colorant Precursor] 1.1 mg of compound (1) was dissolved in 50 mL of tetrahydrofuran (THF) [stabilizer-containing, Wako Grade 1, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.] to prepare a THF solution of compound (1). The prepared THF solution of compound (1) was then placed in a 1 cm cell, and the absorption spectrum was measured using a Shimadzu Corporation ultraviolet-visible spectrophotometer [model: UV-2600] as a measuring device, and the molar absorption coefficient at each wavelength was determined in 1 nm increments. The average molar absorption coefficient was then calculated over any continuous 100 nm range within the wavelength range of 400 nm to 700 nm. The average molar absorption coefficient of compound (2) was also calculated using the same procedure as for compound (1).
[0465] The average molar absorption coefficient of compound (1) was in the range of more than 100 L / (mol cm) to 200 L / (mol cm), and the average molar absorption coefficient of compound (2) was 100 L / (mol cm) or less.
[0466] [Evaluation of Black Color Formation of Colorant Precursor] 1.1 mg of compound (1) was heated in an environment at an ambient temperature of 230°C for 60 minutes to form a black color. The obtained black color form of compound (1) was dissolved in 50 mL of tetrahydrofuran (THF) [containing a stabilizer, Wako Grade 1, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.] to prepare a THF solution of black color form of compound (1). Next, the prepared THF solution of black color form of compound (1) was placed in a 1 cm cell, and the absorption spectrum was measured using a UV-visible spectrophotometer (model number: UV-2600) manufactured by Shimadzu Corporation as a measuring device, and the maximum absorption wavelength and the molar absorption coefficient at the maximum absorption wavelength (however, when there were two or more maximum absorption wavelengths, the molar absorption coefficient at the wavelength with the greatest absorption) were determined. The molar absorption coefficient was also determined in 1 nm increments at each wavelength, and the average molar absorption coefficient was calculated for any consecutive 100 nm range within the wavelength range of 400 nm to 700 nm. The absorption spectrum of compound (2) was also measured using the same procedure as for compound (1), and the maximum absorption wavelength and the molar absorption coefficient at the maximum absorption wavelength (however, if there were two or more maximum absorption wavelengths, the molar absorption coefficient at the wavelength with the greatest absorption) were determined. The average molar absorption coefficient was also calculated for any consecutive 100 nm range within the wavelength range of 400 nm to 700 nm.
[0467] The black colored compound (1) had maximum absorption wavelengths of 422 nm and 681 nm, a molar absorption coefficient at the maximum absorption wavelength of 5900 L / (mol cm), and an average molar absorption coefficient in any continuous 100 nm range of 3000 L / (mol cm) or more. The black colored compound (2) had maximum absorption wavelengths of 419 nm and 677 nm, a molar absorption coefficient at the maximum absorption wavelength of 6300 L / (mol cm), and an average molar absorption coefficient in any continuous 100 nm range of 3000 L / (mol cm).
[0468] [Preparation of Colorant Precursor Dispersions] [D-1 to D-10] The components were mixed to obtain the compositions shown in Table 2. To the resulting mixture, zirconia beads (bead diameter: 0.1 mm) were added in an amount three times the mass of the mixture, and then dispersion was carried out using an MSE (Multi-Stacked Elements) mixer at a peripheral speed of 9 m / s for 90 minutes. After dispersion, the zirconia beads were separated using a filter with a nominal filtration particle size of 73 μm, and colorant precursor dispersions D-1 to D-10 were obtained.
[0469] [Preparation of Colorant Dispersion Liquid] [D-11] The components were mixed to obtain the composition shown in Table 2. To the resulting mixture, zirconia beads (bead diameter: 0.1 mm) in an amount three times the mass of the mixture were added, and then dispersion was carried out using an MSE (Multi-Stacked Elements) mixer at a peripheral speed of 9 m / sec for 90 minutes. After dispersion, the zirconia beads were separated using a filter with a nominal filtration particle size of 73 μm, to obtain Colorant Dispersion Liquid D-11.
[0470]
[0471] In Table 2, "-" means that the corresponding component is not blended. The amine value and acid value of the dispersant shown in Table 2 are catalog values.
[0472] [Preparation of Photosensitive Compositions] [Examples 1A to 10A] The components were mixed to obtain the compositions shown in Table 3, and then stirred for 20 minutes to obtain photosensitive compositions E-1 to E-10 of Examples 1A to 10A.
[0473] Comparative Examples 1A to 3A The components were mixed to obtain the compositions shown in Table 3, and then stirred for 20 minutes to obtain photosensitive compositions E-11 to E-13 of Comparative Examples 1A to 3A.
[0474]
[0475] In Table 3, "-" means that the corresponding component was not blended.
[0476] [Preparation of Transfer Film (1)] [Example 1B] The photosensitive composition E-1 of Example 1A was prepared and then allowed to stand at room temperature (25°C) for 6 hours. After standing, the photosensitive composition E-1 was applied onto a temporary support (trade name: Lumirror (registered trademark) 16KS40, biaxially oriented polyethylene terephthalate (PET) film, thickness: 16 μm, manufactured by Toray Industries, Inc.) using a slit nozzle in an amount to form a coating film with a dry thickness of 15 μm. The solvent in the formed coating film was then evaporated in a drying zone at 100°C to form a photosensitive composition layer. A protective film (trade name: Lumirror (registered trademark) 16KS40, biaxially oriented polyethylene terephthalate (PET) film, thickness: 16 μm, manufactured by Toray Industries, Inc.) was then pressure-bonded onto the formed photosensitive composition layer to prepare the transfer film Y-1 of Example 1B.
[0477] [Examples 2B to 10B] Transfer films Y-2 to Y-10 of Examples 2B to 10B were prepared in the same manner as in Example 1B, except that the type of photosensitive composition was changed to photosensitive compositions E-2 to E-10 of Examples 2A to 10A shown in Table 3.
[0478] Comparative Examples 1B to 3B Transfer films Y-11 to Y-13 of Comparative Examples 1B to 3B were prepared in the same manner as in Example 1B, except that the type of photosensitive composition was changed to photosensitive compositions E-11 to E-13 of Comparative Examples 1A to 3A shown in Table 3.
[0479] [Preparation of a patterned laminate] [Example 1C] After peeling off the protective film from the transfer film Y-1 of Example 1B, the exposed surface of the photosensitive composition layer was laminated to a 50 μm thick PET film [trade name: COSMOSHINE (registered trademark) A4360, manufactured by Toyobo Co., Ltd.] to obtain a laminate having a laminated structure of temporary support / photosensitive composition layer / PET film. The lamination conditions were a roll temperature of 110 ° C, a linear pressure of 0.6 MPa, and a linear speed (so-called lamination speed) of 2 m / min. Next, the prepared laminate was exposed to i-line (wavelength 365 nm) at an exposure dose of 150 mJ / cm using a proximity exposure machine with an ultra-high pressure mercury lamp [manufactured by Hitachi High-Tech Electronics Engineering Co., Ltd.] and a photomask without peeling off the temporary support. 2The photomask had an L (line) / S (space) pattern with line widths varying in 1 μm increments in the range of 1 μm to 100 μm. After exposure, the temporary support of the laminate was peeled off. The laminate was then developed for 30 seconds using a 1% by mass potassium carbonate aqueous solution (liquid temperature: 30°C), rinsed with a shower of pure water, and then dried at 75°C for 13 seconds, thereby developing and removing the photosensitive composition layer in the unexposed areas. Furthermore, the laminate was exposed to i-rays (wavelength 365 nm) at an exposure dose of 1000 mJ / cm. 2 The laminate with the cured photosensitive composition layer was then heat-treated for 5 minutes using a convection oven with the temperature inside set to 210°C, to produce a laminate Z-1 having the pattern of Example 1C.
[0480] [Examples 2C to 10C] Laminates Z-2 to Z-10 having the patterns of Examples 2C to 10C were produced in the same manner as in Example 1C, except that the type of transfer film was changed to transfer films Y-2 to Y-10 of Examples 2B to 10B.
[0481] [Comparative Examples 1C and 2C] The same operations as in Example 1C were carried out except that the type of transfer film was changed to transfer film Y-11 of Comparative Example 1B and transfer film Y-12 of Comparative Example 2B, to prepare laminate Z-11 having the pattern of Comparative Example 1C and laminate Z-12 having the pattern of Comparative Example 2C.
[0482] [Comparative Example 3C] After peeling off the protective film from the transfer film Y-13 of Comparative Example 3B, the exposed surface of the photosensitive composition layer was laminated to a 50 μm thick PET film [trade name: COSMOSHINE (registered trademark) A4360, manufactured by Toyobo Co., Ltd.] to obtain a laminate having a laminated structure of temporary support / photosensitive composition layer / PET film. The lamination conditions were a roll temperature of 110 ° C., a linear pressure of 0.6 MPa, and a linear speed (so-called lamination speed) of 2 m / min. Next, the prepared laminate was exposed to i-line (wavelength 365 nm) at an exposure dose of 150 mJ / cm using a proximity exposure machine with an ultra-high pressure mercury lamp [manufactured by Hitachi High-Tech Electronics Engineering Co., Ltd.] and a photomask without peeling off the temporary support. 2The photomask had an L (line) / S (space) pattern with line widths varying in 1 μm increments in the range of 1 μm to 100 μm. After exposure, the temporary support of the laminate was peeled off. The laminate was then developed for 30 seconds using a 1% by mass potassium carbonate aqueous solution (liquid temperature: 30°C), rinsed with a shower of pure water, and then dried at 75°C for 13 seconds, thereby developing and removing the photosensitive composition layer in the unexposed areas. Furthermore, the laminate was exposed to i-rays (wavelength 365 nm) at an exposure dose of 1000 mJ / cm. 2 The photosensitive composition layer was cured by exposure to light at 1000 K. The laminate with the cured photosensitive composition layer was then immersed in a 10% by mass aqueous hydrochloric acid solution for 20 minutes in an environment with an ambient temperature of 25° C. The laminate was then rinsed with pure water and dried at 75° C. for 13 seconds to produce a laminate Z-13 having the pattern of Comparative Example 3C.
[0483] [Evaluation (1)] The following evaluations were carried out using the photosensitive compositions E-1 to E-10 of Examples 1A to 10A and the photosensitive compositions E-11 to E-13 of Comparative Examples 1A to 3A, the transfer films Y-1 to Y-10 of Examples 1B to 10B and the transfer films Y-11 to Y-13 of Comparative Examples 1B to 3B, and the patterned laminates Z-1 to Z-10 of Examples 1C to 10C and the patterned laminates Z-11 to Z-13 of Comparative Examples 1C to 3C.
[0484] 1. Dispersion Stability The dispersion stability of the colorant precursor in the photosensitive composition was evaluated. When preparing a transfer film, the photosensitive composition used to prepare this transfer film was appropriately diluted with methyl ethyl ketone (MEK), and the particle size distribution of the colorant precursor or colorant contained therein was measured. For the measurement, a laser diffraction / scattering particle size distribution measuring device (model number: LA-960 series) manufactured by Horiba, Ltd. was used. Evaluation was performed according to the following evaluation criteria based on the median diameter (d50: volume-based cumulative 50% diameter) and particle diameter obtained by the measurement. The results are shown in Tables 4 and 5. In the evaluation criteria below, "A," "B," and "C" are practically acceptable levels, with "A" being the most preferable.
[0485] -Evaluation criteria- A: The median diameter (d50) is less than 250 nm, and no particles with a particle diameter of 5000 nm or more are observed. B: The median diameter (d50) is 250 nm or more and less than 500 nm, and no particles with a particle diameter of 5000 nm or more are observed. C: The median diameter (d50) is 500 nm or more and less than 2000 nm, and no particles with a particle diameter of 5000 nm or more are observed. D: Particles with a median diameter (d50) of 2000 nm or more and / or particles with a particle diameter of 5000 nm or more are observed.
[0486] 2. Coloring Stability Over Time The coloring stability of the photosensitive composition over time was evaluated. Photosensitive composition E-13 was not evaluated because it already exhibited a deep black color at the time of preparation. After peeling the protective film from the transfer film, the exposed surface of the photosensitive composition layer was laminated on Gorilla Glass (registered trademark) [thickness: 700 μm, manufactured by Corning Incorporated] to obtain a laminate having a laminate structure of temporary support / photosensitive composition layer / Gorilla Glass. The lamination conditions were a roll temperature of 110°C, a linear pressure of 0.6 MPa, and a linear speed (so-called lamination speed) of 2.0 m / min. The temporary support was peeled from the prepared laminate to prepare Laminate X. The absorbance of the prepared Laminate X at a wavelength of 550 nm was measured using a UV-visible spectrophotometer (model number: UV-2600) manufactured by Shimadzu Corporation. The absorbance value obtained by measurement was divided by the film thickness to determine the absorbance per 1 μm of film thickness at a wavelength of 550 nm (so-called absorption coefficient), and evaluation was performed according to the following evaluation criteria. The results are shown in Tables 4 and 5. In the evaluation criteria below, "A," "B," and "C" indicate practically acceptable levels, with "A" being the most preferable. The lower the absorbance value at a wavelength of 550 nm per 1 μm of film thickness, the less likely the colorant precursor contained in the photosensitive composition is to develop an unintended color before color development due to thermal stimulation, and the more excellent the color stability of the photosensitive composition over time.
[0487] -Evaluation criteria- A: The absorbance per 1 μm of film thickness at a wavelength of 550 nm is less than 0.04. B: The absorbance per 1 μm of film thickness at a wavelength of 550 nm is 0.04 or more and less than 0.07. C: The absorbance per 1 μm of film thickness at a wavelength of 550 nm is 0.07 or more and less than 0.10. D: The absorbance per 1 μm of film thickness at a wavelength of 550 nm is 0.10 or more.
[0488] 3. Aspect Ratio The absorbance of the patterned portion of the laminate having a pattern was measured using a UV-visible spectrophotometer (model number: UV-2600) manufactured by Shimadzu Corporation, and the average absorbance at wavelengths of 400 nm to 600 nm was determined. The average absorbance value was divided by the film thickness of the patterned portion to determine the absorbance per 1 μm of film thickness (the so-called absorption coefficient). As a result, it was confirmed that the absorbance per 1 μm of film thickness was 0.2 or more for the patterned portions of laminates Z-1 to Z-10 having the patterns of Examples 1C to 10C and laminates Z-11 to Z-13 having the patterns of Comparative Examples 1C to 3C. Similarly, the average absorbance at wavelengths of 400 nm to 700 nm was determined. The average absorbance value was divided by the film thickness of the patterned portion to determine the absorbance per 1 μm of film thickness. As a result, it was confirmed that the absorbance per μm of film thickness was 0.20 to 4.0 for all the patterned portions of the laminates Z-1 to Z-10 having the patterns of Examples 1C to 10C. Furthermore, cross-sections of the patterned laminates were observed using a scanning electron microscope (SEM), and the film thickness and minimum resolved line width of the pattern were measured. The "minimum resolved line width" refers to the line width at the bottom of the pattern with the smallest line width among the patterns in which no residue was observed when the space portion was observed with an optical microscope. The aspect ratio was calculated from the measured film thickness and minimum resolved line width of the pattern using the following formula, and evaluation was performed according to the following evaluation criteria. The results are shown in Tables 4 and 5. In the following evaluation criteria, "A," "B," and "C" are practical levels, with "A" being the most preferable. "Aspect ratio" = "film thickness" / "minimum resolved line width"
[0489] -Evaluation criteria- A: The minimum line width is 15 μm or less, and the aspect ratio is 10 or more. B: The minimum line width is 15 μm or less, and the aspect ratio is 5 or more and less than 10. C: The minimum line width is 15 μm or less, and the aspect ratio is 1 or more and less than 5. D: The minimum line width exceeds 15 μm, and / or the aspect ratio is less than 1.
[0490] 4. Photobleaching A black light-shielding tape (trade name: Scotch (registered trademark) Super 88, manufactured by 3M Japan Co., Ltd.) was applied to the PET film side of the patterned laminate to block light. The laminate obtained by this light-shielding process was used as a test sample. Next, the test sample was placed in a highly accelerated weathering tester (trade name: Super Xenon Weather Meter SX75, manufactured by Suga Test Instruments Co., Ltd.) with the patterned surface facing the light source, and subjected to an ambient temperature of 35°C, a relative humidity of 55%, and an illuminance of 0.8 W / m at 420 nm. 2 A 100-hour light resistance test was conducted under the conditions of: After the test, the black light-shielding tape was peeled off from the test sample. The absorbance of the patterned portion was measured using an ultraviolet-visible spectrophotometer (model: UV-2600) manufactured by Shimadzu Corporation, and the average absorbance at wavelengths of 400 nm to 600 nm was determined. The average absorbance value was divided by the film thickness of the patterned portion to determine the average absorbance per μm of film thickness (so-called average absorption coefficient), and evaluation was performed according to the following evaluation criteria. The results are shown in Tables 4 and 5. In the following evaluation criteria, "A," "B," and "C" are practically acceptable levels, with "A" being the most preferable.
[0491] -Evaluation criteria- A: The average absorbance per 1 μm of film thickness at wavelengths of 400 nm to 600 nm is 0.3 or more. B: The average absorbance per 1 μm of film thickness at wavelengths of 400 nm to 600 nm is 0.2 or more and less than 0.3. C: The average absorbance per 1 μm of film thickness at wavelengths of 400 nm to 600 nm is 0.15 or more and less than 0.2. D: The average absorbance per 1 μm of film thickness at wavelengths of 400 nm to 600 nm is less than 0.15.
[0492]
[0493]
[0494] The results shown in Table 4 confirm that photosensitive compositions E-1 to E-10 according to the present disclosure can form black patterns with high aspect ratios. It was also confirmed that photosensitive compositions E-1 to E-10 according to the present disclosure can form black patterns that are resistant to fading by irradiation with a xenon lamp and have excellent lightfastness. It was also confirmed that photosensitive compositions E-1 to E-10 according to the present disclosure have excellent dispersion stability of the colorant precursor, which is a compound represented by formula (1). It was also confirmed that photosensitive compositions E-1 to E-10 according to the present disclosure have excellent color stability over time, with the colorant precursor, which is a compound represented by formula (1), not developing unintended color.
[0495] On the other hand, as shown in Table 5, it was confirmed that a black pattern with a high aspect ratio could not be formed with photosensitive composition E-11 containing a dispersant with an amine value of more than 70 mgKOH / g. It was also confirmed that photosensitive composition E-11 unintentionally developed color from the colorant precursor, which is a compound represented by formula (1), and had poor color stability over time. It was confirmed that a black pattern formed with photosensitive composition E-12 containing a colorant precursor (a so-called leuco dye) that does not fall under the category of a compound represented by formula (1) faded significantly upon irradiation with a xenon lamp, and had poor lightfastness. It was confirmed that a black pattern with a high aspect ratio could not be formed with photosensitive composition E-13 containing carbon black.
[0496] [Preparation of Transfer Films (2)] [Examples 11B to 16B] The same operation as in Example 1B was carried out, except that the photosensitive composition E-1 was applied in an amount adjusted so as to achieve a film thickness after drying as shown in Table 6, to form a photosensitive composition layer, to prepare transfer films Y-14 to Y-19 of Examples 11B to 16B.
[0497] [Fabrication of Micro LED Display Element] [Example 1a] The micro LED display element V-1 of Example 1a was fabricated using the transfer film Y-1 of Example 1B. Specifically, the LED chip was bonded to a bonding member on an array substrate, and then a resin pattern (a so-called partition layer) was formed using the transfer film Y-1. The detailed procedure is shown below.
[0498] The protective film of transfer film Y-1 of Example 1B was peeled off, and the exposed surface of the photosensitive composition layer was attached to an array substrate to which LED chips had been bonded under the lamination conditions shown below, thereby producing a substrate P in which a photosensitive composition layer and a temporary support were laminated in this order on a substrate with light-emitting elements (so-called substrate with chips).
[0499] -Lamination conditions- Heating temperature of chip-attached substrate: 40°C Temperature of rubber roller: 110°C Linear pressure: 3 N / cm Transport speed: 2 m / min
[0500] The distance between the surface of the temporary support provided on the substrate P and the surface of the exposure mask (a mask having a so-called opening formation pattern) was set to 125 μm. Then, using a proximity type exposure machine (manufactured by Hitachi High-Tech Electronics Engineering Co., Ltd.) equipped with an ultra-high pressure mercury lamp, i-rays (wavelength 365 nm) were irradiated at 100 mJ / cm through the temporary support onto the photosensitive composition layer. 2 The substrate was irradiated in a pattern with an exposure dose of 1000 mJ / cm. During this exposure process, the relative positions of the substrate with light-emitting elements and the exposure mask were adjusted while observing the alignment marks previously provided on the substrate with light-emitting elements and the exposure mask with a camera. After the exposure process, the temporary support of the substrate P was peeled off. Next, the exposed photosensitive composition layer was developed for 60 seconds using a 1% by mass aqueous sodium carbonate solution (liquid temperature: 32°C). Next, the residue was removed by spraying ultrapure water from an ultra-high pressure cleaning nozzle onto the laminate obtained after the development process. Thereafter, air was further blown to remove moisture, thereby obtaining a pattern. Next, the obtained pattern was exposed to i-line (wavelength 365 nm) at 1000 mJ / cm using a post-exposure machine (manufactured by Ushio Inc.) equipped with a high-pressure mercury lamp. 2 An exposure treatment (so-called post-exposure) was carried out in which the laminate was irradiated with light at an exposure dose of 1000 kJ / cm 2 (the so-called post-exposure). Next, the laminate after this exposure treatment was subjected to a heat treatment (so-called post-bake treatment) for 5 minutes using a convection oven with the temperature inside set to 210°C. In this manner, a micro LED display element V-1 of Example 1a was produced. In the micro LED display element V-1, a resin pattern having an opening is formed at the position on the array substrate where the LED chip is bonded.
[0501] Examples 1b to 1g Micro LED display elements V-2 to V-7 of Examples 1b to 1g were produced in the same manner as in Example 1a, except that the type of transfer film was changed to transfer films Y-14 to Y-19 of Examples 11B to 16B. Each of the micro LED display elements V-2 to V-7 had a resin pattern with an opening formed at the position where the LED chip was bonded on the array substrate.
[0502] [Evaluation (2)] 1. Light bleeding into adjacent pixels Micro LED display elements V-1 to V-7 of Examples 1a to 1g were used to evaluate light bleeding into adjacent pixels. Using a microscopic ultraviolet-visible-near-infrared spectrophotometer (product name: MSV-5500, manufactured by JASCO Corporation), the light intensity at 530 nm was measured at the position of an adjacent pixel when a green pixel with a central emission wavelength of 530 nm was made to emit light. The light intensity at 530 nm at the adjacent pixel was calculated when the light intensity at 530 nm at the emitting pixel was taken as 100%, and evaluation was performed according to the following evaluation criteria. The results are shown in Table 6. In the evaluation criteria below, "A," "B," and "C" represent practically acceptable levels, with "A" being the most preferable.
[0503] -Evaluation criteria- A: The light intensity at 530 nm in adjacent pixels is less than 0.01%. B: The light intensity at 530 nm in adjacent pixels is 0.01% or more and less than 0.1%. C: The light intensity at 530 nm in adjacent pixels is 0.1% or more and less than 1%. D: The light intensity at 530 nm in adjacent pixels is 1% or more.
[0504]
[0505] "Y-1" in Table 6 is the same as "Y-1" in Table 4. Also, "E-1" in Table 6 is the same as "E-1" in Tables 3 and 4.
[0506] The results shown in Table 6 confirm that when a black pattern having a film thickness of 5 μm or more formed using the photosensitive composition according to the present disclosure is used as a partition wall, light leakage to adjacent pixels is effectively suppressed.
[0507] The disclosures of Japanese Patent Applications Nos. 2023-056659 and 2023-111021 are incorporated herein by reference in their entirety. Furthermore, all documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually indicated to be incorporated by reference.
Claims
1. A photosensitive composition comprising: a compound represented by the following formula (1) which is a colorant precursor; and a dispersant having an amine value of 70 mgKOH / g or less. In formula (1), X 1 , X 2 , X 3 , X 4 , Y 1 and Y 2 each independently represents an oxygen atom, a sulfur atom, or N-L 1 Represents: L 1 R represents a hydrogen atom, an alkyl group, an acyl group, an alkoxycarbonyl group, or an aminocarbonyl group. 1 , R 2 , R 3 and R 4 each independently represents a hydrogen atom, -O-L 2 , -OCO-L 3 , -S-L 2 Or -OSO-L 3 Represents: L 2 represents a hydrogen atom or an alkyl group; L 3 represents an alkyl group or an amino group. 1 and R 2 At least one of represents a hydrogen atom, and R 3 and R 4 At least one of A, B and C independently represents an aromatic ring.
2. The photosensitive composition according to claim 1, wherein the acid value of said dispersing agent is 15 mg KOH / g or more.
3. The photosensitive composition according to claim 1, further comprising an alkali-soluble resin, a polymerizable monomer and a photopolymerization initiator.
4. A method for producing a photosensitive composition, comprising: preparing a dispersion liquid containing a compound represented by the following formula (1) which is a colorant precursor, a dispersant having an amine value of 70 mgKOH / g or less, and a solvent; and mixing the dispersion liquid with an alkali-soluble resin, a polymerizable monomer, and a photopolymerization initiator. In formula (1), X 1 , X 2 , X 3 , X 4 , Y 1 and Y 2each independently represents an oxygen atom, a sulfur atom, or N-L 1 Represents: L 1 represents a hydrogen atom, an alkyl group, an acyl group, an alkoxycarbonyl group, or an aminocarbonyl group. 1 , R 2 , R 3 and R 4 each independently represents a hydrogen atom, -O-L 2 , -OCO-L 3 , -S-L 2 Or -OSO-L 3 Represents: L 2 represents a hydrogen atom or an alkyl group; L 3 represents an alkyl group or an amino group. 1 and R 2 At least one of R represents a hydrogen atom; 3 and R 4 At least one of A, B and C independently represents an aromatic ring.
5. A transfer film comprising: a temporary support; and a photosensitive composition layer containing the photosensitive composition according to any one of claims 1 to 3.
6. A method for producing a laminate having a black pattern, comprising the steps of: forming a photosensitive composition layer containing the photosensitive composition according to any one of claims 1 to 3 on a substrate; exposing the photosensitive composition layer to pattern light; and developing the photosensitive composition layer, in this order; and further comprising, after the step of exposing the photosensitive composition to pattern light, causing the compound represented by formula (1) to develop a black color.
7. A laminate having a black pattern, produced by the method of claim 6.
8. The laminate according to claim 7, wherein the black pattern has an aspect ratio, which is the ratio of the film thickness to the bottom line width, of 1 or more.
9. The laminate according to claim 7, wherein the black pattern satisfies the relationship 0.15≦X / Y, where X is the average absorbance at wavelengths of 400 nm to 600 nm and Y μm is the film thickness.
Citation Information