Curable composition

The curable composition, featuring an organic polymer with a difunctional dialkoxysilyl group, amidine and titanium compounds, and a specific silane condensate, overcomes the slow curing challenge in curable compositions, achieving faster curing speeds.

WO2024203438A1PCT designated stage expired Publication Date: 2024-10-03KANEKA CORP
View PDF 32 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010176
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-15
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Curable compositions containing organic polymers with reactive silicon groups face challenges in achieving fast curing rates when using non-tin catalysts, particularly when combined with difunctional dialkoxylyl groups, resulting in insufficient curing speed.

Method used

A curable composition comprising an organic polymer with a difunctional dialkoxysilyl group, a silane compound, and a curing catalyst system that includes an amidine compound and a titanium compound, along with a specific silane condensate, is developed to enhance curing speed.

Benefits of technology

The combination of amidine and titanium compounds with a silane condensate significantly improves the curing speed of the curable composition, addressing the slow curing issues associated with non-tin catalysts and difunctional dialkoxylyl groups.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The present invention provides a curable composition that contains a silane compound, a non-tin-based curing catalyst, and an organic polymer having a bifunctional dialkoxysilyl group as a reactive silicon group, and that exhibits quick curability. Provided is a curable composition that contains a silane compound, a non-tin-based curing catalyst, and an organic polymer having a bifunctional dialkoxysilyl group as a reactive silicon group, wherein an amidine compound and a titanium compound are used in combination as the curing catalyst, and a silane condensate having a specific structure is used as the silane compound.
Need to check novelty before this filing date? Find Prior Art

Description

curable composition

[0001] The present invention relates to a curable composition comprising an organic polymer having a reactive silicon group, a curing catalyst containing a specific compound, and a silane condensate.

[0002] Organic polymers having at least one reactive silicon group in the molecule can be crosslinked even at room temperature by forming siloxane bonds accompanied by hydrolysis of the silyl groups due to moisture, etc. It is known that organic polymers having reactive silicon groups have the property of giving rubber-like cured products through such crosslinking reactions.

[0003] When an organic polymer having a reactive silicon group is used as a curable composition for a sealing material, adhesive, paint, waterproofing material, or the like, various properties are required of the curable composition, such as curability, adhesiveness, workability, mechanical properties of the cured product, and waterproofness.

[0004] Curable compositions containing organic polymers having reactive silicon groups are typically cured using a silanol condensation catalyst, such as an organotin compound having a carbon-tin bond, such as dibutyltin bis(acetylacetonate). Silanol condensation catalysts are also called curing catalysts. In recent years, the toxicity of organotin compounds has been highlighted, and the use of non-tin catalysts has been proposed (Patent Document 1).

[0005] JP 2014-114434 A

[0006] In curable compositions containing organic polymers having reactive silicon groups, bifunctional dialkoxysilyl groups such as dimethoxymethylsilyl groups are sometimes used as reactive silicon groups to obtain cured products with high elongation and flexibility. Furthermore, various silane compounds, such as silane coupling agents, may be blended into curable compositions containing organic polymers having reactive silicon groups to improve the stability of the curable compositions or to impart adhesion to substrates. However, organic polymers having bifunctional dialkoxysilyl groups such as dimethoxymethylsilyl groups generally have low hydrolysis resistance. In particular, when organic polymers having bifunctional dialkoxysilyl groups are combined with non-tin catalysts, a problem arises in that a sufficient curing rate cannot be achieved. Patent Document 1 proposes the use of a combination of DBU and diisopropoxytitanium bis(ethylacetoacetate) as a non-tin curing catalyst in a curable composition containing a trimethoxysilane coupling agent and an organic polymer having dimethoxymethylsilyl groups. However, the curing rate of the curable composition described in Patent Document 1 was insufficient. Therefore, there is a demand for an improvement in the curing speed of a curable composition containing an organic polymer having a bifunctional dialkoxysilyl group, a silane compound, and a non-tin curing catalyst.

[0007] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a curable composition that exhibits fast curing properties, which comprises an organic polymer having a bifunctional dialkoxysilyl group as a reactive silicon group, a silane compound, and a non-tin curing catalyst.

[0008] In order to solve the above problems, the present inventors discovered that the above problems can be solved by using a combination of an amidine compound and a titanium compound as the curing catalyst and a silane condensate having a specific structure as the silane compound in a curable composition containing an organic polymer having a bifunctional dialkoxysilyl group as the reactive silicon group, a silane compound, and a non-tin curing catalyst, and thus completed the present invention.

[0009] That is, the present invention provides a curable composition comprising an organic polymer (A), a curing catalyst (B), and a silane condensate (C), wherein the organic polymer (A) is a silane represented by the following formula (1): -SiR 1 X 2 (1) (In formula (1), R 1 is a hydrocarbon group having 1 to 20 carbon atoms, X is a hydroxyl group or a hydrolyzable group, and two Xs may be the same or different. The curing catalyst (B) contains an amidine compound (b1) and a titanium compound (b2), and the amidine compound (b1) is a compound represented by the following formula (2): R 2 N=CR 3 -NR 4 2 (2) (In formula (2), R 2 , R 3 , and R 4 is a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, and two R 4 may be the same or different, and R 2 , R 3 , and two R 4 Any two of these may be bonded to form a ring, and the titanium compound (b2) is a compound represented by the following formula (3): Ti(OR 5 ) d Y 4-d (3) (In formula (3), R 5 is a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, Y is a chelate coordination compound, and d is an integer of 0 to 4, or a condensate thereof, and the silane condensate (C) is a compound represented by the following formula (4): (In formula (4), R 6 is a methyl group or an ethyl group, and R 6 may be the same or different, R 7 , R 8 is a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, and R 7 , R 8 may be the same or different, and e and f are integers of 1 to 50.

[0010] According to the present invention, it is possible to provide a curable composition that exhibits fast curing properties, which comprises an organic polymer having a bifunctional dialkoxysilyl group as a reactive silicon group, a silane compound, and a non-tin curing catalyst.

[0011] The present invention will be described in detail below.

[0012] <Curable Composition> The curable composition contains an organic polymer (A), a curing catalyst (B), and a silane condensate (C). The organic polymer (A) has a reactive silicon group represented by the following formula (1): —SiR 1 X 2 (1)

[0013] In formula (1), R 1 is a hydrocarbon group having 1 to 20 carbon atoms. X is a hydroxyl group or a hydrolyzable group. The two Xs may be the same or different.

[0014] The curing catalyst (B) contains an amidine compound (b1) and a titanium compound (b2). The amidine compound (b1) is a compound represented by the following formula (2): 2 N=CR 3 -NR 4 2 (2)

[0015] In formula (2), R 2 , R 3 , and R 4 is a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent. 4 may be the same or different. 2 , R 3 , and two R 4 Any two of these may be bonded to form a ring.

[0016] The titanium compound (b2) is a compound represented by the following formula (3) or a condensate thereof: Ti(OR 5 ) d Y 4-d (3)

[0017] In formula (3), R 5represents a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent; Y represents a chelate coordination compound; and d represents an integer of 0 to 4.

[0018] The silane condensate (C) is a compound represented by the following formula (4).

[0019] In formula (4), R 6 is a methyl group or an ethyl group, and R 6 may be the same or different. 7 , R 8 is a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, and R 7 , R 8 may be the same or different, and e and f are integers of 1 to 50.

[0020] The curable composition may also contain various other additives, if desired.

[0021] Essential and optional components that the curable composition may contain are described below.

[0022] <Organic Polymer (A)> The organic polymer (A) has a reactive silicon group represented by the above formula (1). The organic polymer (A) has a polymer backbone and a polymer chain end bonded to the polymer backbone. In the specification and claims of this application, the polymer backbone is also referred to as a "main chain structure." The polymer backbone is a structure in which multiple structural units derived from monomers are bonded in succession. The monomer may be of one type or multiple types.

[0023] The polymer chain end is a moiety located at the end of the organic polymer (A). The number of polymer chain ends of the organic polymer (A) is 2 when the main chain structure is linear, and 3 or more when the polymer backbone is branched. When the organic polymer (A) is a mixture of a polymer having a linear main chain structure and a polymer having a branched main chain structure, the number of polymer chain ends is a value between 2 and 3 on average.

[0024] The reactive silicon group may be present in the polymer backbone and at the polymer chain terminal. Two or more reactive silicon groups may be present at the polymer chain terminal. When the curable composition is used for adhesives, sealants, elastic coating agents, pressure-sensitive adhesives, etc., it is preferred that the reactive silicon group in the organic polymer (A) be present at the polymer chain terminal.

[0025] (Reactive silicon group) The reactive silicon group is a group that can generate a silanol group by hydrolysis. When the reactive silicon group generates a silanol group, the organic polymer (A) is crosslinked by a condensation reaction between the silanol groups. As described above, the reactive silicon group is a group represented by the following formula (1): -SiR 1 X 2 (1)

[0026] In formula (1), R 1 is a hydrocarbon group having 1 to 20 carbon atoms. X is a hydroxyl group or a hydrolyzable group, and two Xs may be the same or different.

[0027] R in formula (1) 1 Specific examples of the alkyl group include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-hexyl, 2-ethylhexyl, and n-dodecyl; unsaturated hydrocarbon groups such as vinyl, isopropenyl, and allyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl, toluoyl, and 1-naphthyl; and aralkyl groups such as benzyl. Of these groups, alkyl and aryl groups are preferred, with methyl, ethyl, and phenyl groups being more preferred, methyl and ethyl groups being even more preferred, and methyl being particularly preferred.

[0028] X in formula (1) is a hydroxyl group or a hydrolyzable group. The hydrolyzable group is not particularly limited and may be a known hydrolyzable group. Specific examples of the hydrolyzable group include a hydrogen atom, a halogen atom, an alkoxy group, an acyloxy group, a ketoximate group, an amino group, an amide group, an acid amide group, an aminooxy group, a mercapto group, and an alkenyloxy group. Among these, an alkoxy group, an acyloxy group, a ketoximate group, and an alkenyloxy group are preferred, and an alkoxy group such as a methoxy group and an ethoxy group is more preferred because of its mild hydrolysis and ease of handling. The two Xs in formula (1) may be the same group or different groups.

[0029] The reactive silicon group represented by formula (1) is not particularly limited. Specific examples of the reactive silicon group represented by formula (1) include a dimethoxymethylsilyl group, a diethoxymethylsilyl group, and a dimethoxyphenylsilyl group. Among these, a dimethoxymethylsilyl group is preferred because the raw material is easily available.

[0030] (Regarding the Main Chain Structure of the Organic Polymer (A)) The main chain structure of the organic polymer (A) is not particularly limited and may be any of various known main chain structures. Specific examples of the main chain structure include polyoxyalkylene polymers such as polyoxyethylene polymers, polyoxypropylene polymers, polyoxybutylene polymers, polyoxytetramethylene polymers, polyoxyethylene-polyoxypropylene copolymers, and polyoxypropylene-polyoxybutylene copolymers; hydrocarbon polymers such as ethylene-propylene copolymers, polyisobutylene, isobutylene-isoprene copolymers, polybutadiene, and hydrogenated polyolefin polymers obtained by hydrogenating these polyolefin polymers; polycondensates of dibasic acids such as adipic acid and glycols; and ring-opening polymers of lactones; (meth)acrylic acid ester polymers obtained by radical polymerization of (meth)acrylic acid ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and stearyl (meth)acrylate; vinyl copolymers obtained by radical polymerization of two or more monomers selected from (meth)acrylic acid ester monomers, vinyl acetate, acrylonitrile, and styrene; polysulfide polymers; diallyl phthalate polymers, etc. Note that (meth)acrylic acid ester refers to both acrylic acid esters and methacrylic acid esters.

[0031] As the main chain structure, polyoxyalkylene polymers and (meth)acrylic acid ester polymers are particularly preferred because they have excellent deep curing properties as a one-component composition due to their high moisture permeability and also excellent adhesiveness. As the main chain structure, polyoxyalkylene polymers are more preferred, and polyoxypropylene is even more preferred.

[0032] The polyoxyalkylene polymer is -R 9 It is a polymer having a repeating unit represented by —O—. 9 is a linear or branched alkylene group having 1 to 14 carbon atoms. 9 is more preferably a linear or branched alkylene group having 2 to 4 carbon atoms.9 Specific examples of the repeating unit represented by —O— include —CH 2 O-, -CH 2 CH 2 O-, -CH 2 CH (CH 3 ) O—, —CH 2 CH(C 2 H 5 ) O—, —CH 2 C(CH 3 ) (CH 3 ) O—, and —CH 2 CH 2 CH 2 CH 2 O-, etc. The main chain structure of the polyoxyalkylene polymer may consist of only one type of repeating unit, or may consist of two or more types of repeating units. In particular, when the curable composition is used as a sealant, adhesive, etc., a polyoxypropylene polymer having oxypropylene repeating units in an amount of 50% by weight or more, preferably 80% by weight or more, of the polymer main chain structure is preferred as the polyoxyalkylene polymer. This is because such polyoxyalkylene polymers are amorphous and have relatively low viscosity.

[0033] The main chain structure of the polyoxyalkylene polymer may be linear or branched.

[0034] The polyoxyalkylene polymer is preferably a polymer obtained by ring-opening polymerization of a cyclic ether compound in the presence of an initiator using a polymerization catalyst.

[0035] Examples of cyclic ether compounds include ethylene oxide, propylene oxide, butylene oxide, tetramethylene oxide, and tetrahydrofuran. These cyclic ether compounds may be used alone or in combination of two or more. Among these cyclic ether compounds, propylene oxide is particularly preferred because it can produce an amorphous polyether polymer with a relatively low viscosity.

[0036] Specific examples of the initiator include alcohols such as butanol, ethylene glycol, propylene glycol, propylene glycol monoalkyl ether, butanediol, hexamethylene glycol, neopentyl glycol, diethylene glycol, dipropylene glycol, triethylene glycol, glycerin, trimethylolmethane, trimethylolpropane, pentaerythritol, and sorbitol; and polyoxyalkylene polymers such as polyoxypropylene diol, polyoxypropylene triol, polyoxyethylene diol, and polyoxyethylene triol.

[0037] The method for synthesizing the polyoxyalkylene polymer is not particularly limited. Examples of methods for synthesizing polyoxyalkylene polymers include a polymerization method using an alkali catalyst such as KOH, a polymerization method using a transition metal compound-porphyrin complex catalyst such as the complex obtained by reacting an organoaluminum compound with porphyrin disclosed in JP-A-61-215623, a polymerization method using a composite metal cyanide complex catalyst disclosed in JP-B-46-27250, JP-B-59-15336, U.S. Pat. Nos. 3,278,457, 3,278,458, 3,278,459, 3,427,256, 3,427,334, and 3,427,335, a polymerization method using a catalyst made of a polyphosphazene salt exemplified in JP-A-10-273512, and a polymerization method using a catalyst made of a phosphazene compound exemplified in JP-A-11-060722. The polymerization method using a composite metal cyanide complex catalyst is more preferred because it has low production costs and can produce a polymer with a narrow molecular weight distribution.

[0038] The main chain structure of the organic polymer (A) may be a polyoxyalkylene polymer containing bonds other than ether bonds, such as urethane bonds and urea bonds, within the range that does not significantly impair the desired effects. Specific examples of polymers having such a main chain structure include polyurethane prepolymers and polyurea prepolymers.

[0039] The polyurethane prepolymer can be obtained by a known method such as a method of reacting a polyol compound with a polyisocyanate compound. The polyurea prepolymer can be obtained by a known method such as a method of reacting a polyamine compound with a polyisocyanate compound. The main chain structure may be a prepolymer having a combination of urethane bonds and urea bonds, which is obtained by reacting a polyol compound and a polyamine compound with a polyisocyanate compound.

[0040] Specific examples of the polyol compound include polyether polyol, polyester polyol, polycarbonate polyol, and polyether polyester polyol.

[0041] Specific examples of polyisocyanate compounds include diphenylmethane diisocyanate, tolylene diisocyanate, xylylene diisocyanate, methylene-bis(cyclohexyl isocyanate), isophorone diisocyanate, and hexamethylene diisocyanate.

[0042] The polyurethane prepolymer may have a terminal group of either a hydroxyl group or an isocyanate group, and the polyurea prepolymer may have a terminal group of either an amino group or an isocyanate group.

[0043] In a cured product of a curable composition containing, as the organic polymer (A), a polymer having one or more bonds selected from a urethane bond, a urea bond, and an ester bond in the main chain structure, the strength of the cured product may decrease due to cleavage of the urethane bond, urea bond, or ester bond in the main chain structure due to heat or the like.

[0044] When a polymer containing an amide bond in the main chain structure is used as the organic polymer, the curability of the curable composition may be improved. 10 Represented by -C(=O)-. 10is a hydrogen atom or an organic group which may have a substituent. When the amount of amide bonds in the main chain structure is within an appropriate range, the viscosity of the polymer is low, and a decrease in strength of the cured product due to cleavage of the amide bonds due to heat or the like and an increase in viscosity of the curable composition due to storage are unlikely to occur, and the workability of the curable composition is good.

[0045] When the organic polymer (A) contains an amide bond in its main chain structure, the average number of amide bonds per molecule is preferably 1 to 10, more preferably 1.5 to 5, and even more preferably 2 to 3. When the average number of amide bonds per molecule is within this range, the curable composition has good curability, the organic polymer (A) has a low viscosity, and the organic polymer (A) and the curable composition are easy to handle.

[0046] As the polymer (A) described above, a polyoxyalkylene polymer that does not contain a urethane bond, a urea bond, an ester bond, or an amide bond in the main chain structure is most preferred, from the viewpoint of obtaining a curable composition excellent in storage stability and workability.

[0047] The organic polymer (A) is preferably a polymer obtained by introducing reactive silicon groups into a polymer by any of the following methods (a) to (d): (a) converting the terminal hydroxyl groups of a hydroxyl-terminated organic polymer into carbon-carbon unsaturated groups, and then converting the carbon-carbon unsaturated groups into HSiR 1 X 2 A method of hydrosilylation using a hydrosilane represented by the formula: R 1 and X are the same as those in formula (1). (b) OCN-W-SiR 1 X 2 A method of reacting an isocyanate alkylsilane compound represented by the formula: W is a divalent organic group. 1 and X are the same as those in formula (1). (c) After converting the terminal hydroxyl groups of the hydroxyl-terminated organic polymer into carbon-carbon unsaturated groups, the carbon-carbon unsaturated groups and HS-W-SiR 1 X 2 A method of carrying out an ene-thiol reaction with a mercaptoalkylsilane compound represented by the formula: W is a divalent organic group. 1and X are the same as those in formula (1). (d) A hydroxyl-terminated organic polymer is reacted with a polyisocyanate compound to synthesize an NCO-terminated organic polymer, and then the terminal NCO groups are converted to the corresponding NCO groups by the reaction of HNR 11 -W-SiR 1 X 2 , or HS-W-SiR 1 X 2 A method of reacting a silane compound represented by the formula: W is a divalent organic group. 11 is a hydrogen atom or an alkyl group. 1 , and X are the same as those in formula (1).

[0048] In the above methods (a) and (c), examples of the terminal carbon-carbon unsaturated group include a vinyl group, an allyl group, a methallyl group, an allenyl group, and a propargyl group.

[0049] In any of the above methods (b) to (d), the polymer (A) obtained by using a silane compound in which W is methylene exhibits very high curability.

[0050] The method (a) is preferred because it is easy to obtain an organic polymer (A) having good storage stability, while the methods (b), (c), and (d) are preferred because they can achieve a high conversion rate in a relatively short reaction time.

[0051] The method for introducing reactive silicon groups by method (a) has been proposed in Japanese Patent Publication Nos. 45-36319, 46-12154, Japanese Patent Laid-Open Nos. 50-156599, 54-6096, 55-13767, 55-13468, 57-164123, Japanese Patent Publication No. 3-2450, U.S. Pat. Nos. 3,632,557, 4,345,053, 4,366,307, and 4,960,844. Examples of such methods include the method proposed in JP-A Nos. 61-197631, 61-215622, 61-215623, and 61-218632, in which reactive silicon groups are introduced by hydrosilylation or the like into a polyoxypropylene polymer having a high molecular weight and narrow molecular weight distribution, with a number average molecular weight of 6,000 or more and an Mw / Mn ratio of 1.6 or less, and the method proposed in JP-A No. 3-72527.

[0052] The number average molecular weight of the organic polymer (A) is not particularly limited. The number average molecular weight of the organic polymer (A), as a polystyrene-equivalent molecular weight measured by GPC, is preferably 3,000 to 100,000, more preferably 3,000 to 50,000, and particularly preferably 3,000 to 30,000. When the number average molecular weight is within the above range, the amount of reactive silicon groups introduced is appropriate, making it easy to obtain an organic polymer (A) that has a viscosity that is easy to handle and excellent workability, while keeping production costs within an appropriate range.

[0053] The molecular weight of the organic polymer (A) can also be expressed as an end-group-converted molecular weight calculated by directly measuring the end-group concentration of a polymer precursor before the introduction of reactive silicon groups by titration analysis based on the principles of the hydroxyl value measurement method specified in JIS K 1557 and the iodine value measurement method specified in JIS K 0070, and taking into account the structure of the polymer (the degree of branching determined by the polymerization initiator used). The end-group-converted molecular weight of the organic polymer (A) can also be calculated by preparing a calibration curve of the number average molecular weight determined by general GPC measurement of the polymer precursor and the end-group-converted molecular weight, and converting the number average molecular weight determined by GPC of the organic polymer (A) into an end-group-converted molecular weight.

[0054] The molecular weight distribution (Mw / Mn) of the organic polymer (A) is not particularly limited. It is preferable that the molecular weight distribution of the organic polymer (A) is narrow. Specifically, the molecular weight distribution is preferably 1.6 or less, more preferably 1.4 or less, even more preferably 1.3 or less, and particularly preferably 1.2 or less. The molecular weight distribution of the organic polymer (A) can be determined from the number average molecular weight and weight average molecular weight obtained by GPC measurement.

[0055] In order to obtain a good rubber-like cured product, the reactive silicon groups of the organic polymer (A) are preferably present at the polymer chain terminals. The number of reactive silicon groups per polymer chain terminal is preferably 0.5 or more on average, more preferably 0.6 or more, even more preferably 0.7 or more, and particularly preferably 0.8 or more. When the number of reactive silicon groups is 0.5 or more, the curability of the organic polymer (A) and the curable composition is good, and the cured product of the curable composition has good rubber elasticity.

[0056] The number of reactive silicon groups in one molecule is preferably 1 to 7 on average, more preferably 1 to 4, and particularly preferably 1 to 3.

[0057] Furthermore, as described in WO 2013 / 180203, an organic polymer having two or more reactive silicon groups at the polymer chain terminals can also be used as the organic polymer (A). Such an organic polymer (A) exhibits high curability, and the resulting cured product can be expected to have high strength and high recovery.

[0058] Specific examples of commercially available organic polymers (A) include various reactive silicon group-containing polyoxypropylene products such as Kaneka MS Polymer (registered trademark) and Kaneka Silyl (registered trademark), reactive silicon group-containing poly(meth)acrylic acid ester products such as Kaneka TA Polymer (registered trademark) and KANEKA XMAP (registered trademark), and reactive silicon group-containing polyisobutylene products such as EPION (registered trademark). All of these commercially available organic polymers (A) are products of Kaneka Corporation.

[0059] <Curing Catalyst (B)> The curable composition contains a curing catalyst (B) that cures the organic polymer (A) through hydrolysis condensation. The curing catalyst (B) contains an amidine compound (b1) and a titanium compound (b2).

[0060] (Amidine Compound (b1)) The amidine compound (b1) is a compound represented by the following formula (2): 2 N=CR 3 -NR 4 2 (2)

[0061] In formula (2), R 2 , R 3 , and R 4 is a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent. 4 may be the same or different. 2 , R 3 , and two R 4Any two of these may be bonded to form a ring. When hydrocarbon groups which may have a substituent are bonded to each other to form a ring, one hydrogen atom is removed from each of the two hydrocarbon groups which may have a substituent, and the atoms to which the removed hydrogen atoms on the hydrocarbon groups which may have a substituent are bonded are connected by a single bond to form a ring. When the hydrocarbon group has a substituent, a hydrogen atom bonded to a heteroatom such as a nitrogen atom or oxygen atom contained in the substituent may be removed. When a hydrogen atom and a hydrocarbon group which may have a substituent are bonded to form a ring, R 3 is a hydrogen atom, and R 4 Here, the case where R is a hydrocarbon group which may have a substituent will be described as an example. 3 and one hydrogen atom on the hydrocarbon group which may have a substituent, and R 3 The carbon atom to which the hydrogen atom of R was bonded 4 A ring is formed by connecting the atom to which the removed hydrogen atom on the hydrocarbon group, which may have a substituent as R, via a single bond. 2 , R 3 , and two R 4 When any two of these are bonded to form a ring, for example, R 2 and one R 4 and bond to form a ring, and R 3 and the other R 4 may be bonded to form a ring, and R 2 and R 3 and form a ring, and two R 4 may form a ring.

[0062] R 2 , R 3 , and R 4 The hydrocarbon group represented by R may have a substituent. 2 , R 3 , and R 4 Examples of the substituent that the hydrocarbon group as R may have include a halogen atom, an amino group, an alkylamino group having 1 to 4 carbon atoms, a dialkylamino group having 2 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, and a hydroxyl group.2 , R 3 , and R 4 The number of carbon atoms of the hydrocarbon group as R, excluding the number of carbon atoms of the substituent, is preferably 1 to 12, more preferably 1 to 6, and even more preferably 1 to 4. 2 , R 3 、 and R 4 Specific examples of the hydrocarbon group are the above-mentioned R 1 The specific examples of the hydrocarbon group are the same as those of R. 1 Also preferred are groups in which the groups exemplified as the hydrocarbon groups as R are substituted with the above-mentioned substituents. 2 , R 3 , and two R 4 The ring formed by bonding two of these may be a five-membered ring, a six-membered ring, or a seven-membered ring, preferably a six-membered ring or a seven-membered ring. As the amidine compound (b1), an amidine containing at least one ring structure (i.e., a cyclic amidine) is preferred, and a cyclic amidine containing two ring structures (i.e., a bicyclic amidine) is more preferred.

[0063] Specific examples of the amidine compound include cyclic amidines such as 1,2-dimethyl-1,4,5,6-tetrahydropyrimidine, 1-ethyl-2-methyl-1,4,5,6-tetrahydropyrimidine, 1,2-diethyl-1,4,5,6-tetrahydropyrimidine, 1-n-propyl-2-methyl-1,4,5,6-tetrahydropyrimidine, 1-isopropyl-2-methyl-1,4,5,6-tetrahydropyrimidine, 1-ethyl-2-n-propyl-1,4,5,6-tetrahydropyrimidine, and 1-ethyl-2-isopropyl-1,4,5,6-tetrahydropyrimidine; bicyclic amidines such as DBU (1,8-diazabicyclo[5.4.0]-7-undecene) and DBN (1,5-diazabicyclo[4.3.0]-5-nonene);Guanidine, dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, 1,1-dimethylguanidine, 1,3-dimethylguanidine, 1,2-diphenylguanidine, 1,1,2-trimethylguanidine, 1,2,3-trimethylguanidine, 1,1,3,3-tetramethylguanidine, 1,1,2,3,3-pentamethylguanidine, 2-ethyl-1,1,3,3-tetramethylguanidine, 1,1,3,3-tetramethyl-2-n-propylguanidine, 1,1,3,3-tetramethyl-2-isopropylguanidine, 2-n-butyl-1,1,3,3-tetramethylguanidine, 2-tert-butyl-1,1,3,3-tetramethylguanidine 1,2,3-tricyclohexylguanidine, 1-benzyl-2,3-dimethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-ethyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-n-propyl-1,5,7-triazabicyclo[4.4 guanidines such as 7-isopropyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-n-butyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-cyclohexyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, and 7-n-octyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene;Biguanide, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-(2-ethylhexyl)biguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, 1-(o-tolyl)biguanide, 1-morpholinobiguanide biguanide compounds such as 1-n-butyl-N2-ethylbiguanide, 1,1'-ethylenebisbiguanide, 1,5-ethylenebiguanide, 1-[3-(diethylamino)propyl]biguanide, 1-[3-(dibutylamino)propyl]biguanide, and N',N''-dihexyl-3,12-diimino-2,4,11,13-tetraazatetradecanediamidine;

[0064] In terms of non-bleeding properties, the amount of the amidine compound (b1) used is preferably 0.1 to 4.0 parts by weight, more preferably 0.2 to 3.0 parts by weight, and even more preferably 0.3 to 2.0 parts by weight, per 100 parts by weight of the organic polymer (A).

[0065] (Titanium Compound (b2)) The titanium compound (b2) is a compound represented by the following formula (3): Ti(OR 5 ) d Y 4-d (3)

[0066] In formula (3), R 5 is a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent. Y is a chelate coordination compound. d is an integer of 0 to 4. R 5 The hydrocarbon group as R may be an aliphatic hydrocarbon group or an aromatic hydrocarbon group. 5 When the hydrocarbon group represented by R is an aliphatic hydrocarbon group, the aliphatic hydrocarbon group may have one or more unsaturated bonds. 5 When the hydrocarbon group represented by R is an aliphatic hydrocarbon group, the structure of the aliphatic hydrocarbon group may be linear, branched, or cyclic, or may be a combination of these structures. 5 The hydrocarbon group represented by R may have a substituent. 5 The hydrocarbon group as R preferably has no substituent.5 Examples of the substituents that the hydrocarbon group may have are R 2 , R 3 , and R 4 The examples of the substituents that may be possessed by the hydrocarbon group are the same as those of R 5 The hydrocarbon group represented by R preferably has 1 to 12 carbon atoms, more preferably 1 to 6 carbon atoms, and even more preferably 1 to 4 carbon atoms. 5 Preferred hydrocarbon groups for are methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, and phenyl.

[0067] The chelating coordination compound represented by Y is preferably a bidentate organic ligand. Examples of the chelating coordination compound include β-diketones and β-ketoesters. Specific examples of β-diketones include acetylacetone (ACAC), trifluoroacetylacetone, hexafluoroacetylacetone, benzoylacetone, thenoyltrifluoroacetone, dipivaloylmethane, dibenzoylmethane, and ascorbic acid. Specific examples of β-ketoesters include methyl acetoacetate, ethyl acetoacetate, allyl acetoacetate, benzyl acetoacetate, n-propyl acetoacetate, isopropyl acetoacetate, n-butyl acetoacetate, isobutyl acetoacetate, tert-butyl acetoacetate, 2-methoxyethyl acetoacetate, and methyl 3-oxopentanoate.

[0068] Specific examples of the titanium compound (b2) include tetramethoxytitanium, trimethoxyethoxytitanium, trimethoxyisopropoxytitanium, trimethoxybutoxytitanium, dimethoxydiethoxytitanium, dimethoxydiisopropoxytitanium, dimethoxydibutoxytitanium, methoxytriethoxytitanium, methoxytriisopropoxytitanium, methoxytributoxytitanium, tetraethoxytitanium, triethoxyisopropoxytitanium, triethoxybutoxytitanium, diethoxydiisopropoxytitanium, diethoxydibutoxytitanium, ethoxytriisopropoxytitanium, ethoxytributoxytitanium, tetraisopropoxytitanium, triisopropoxybutoxytitanium, diisopropoxydibutoxytitanium, tetrabutoxytitanium, tetra-tert-butoxytitanium, bis(acetylacetonato)diisopropoxytitanium, bis(ethylacetoacetate)diisopropoxytitanium, and bis(ethylacetoacetate)diisobutoxytitanium. Condensates thereof can also be used as the titanium compound (b2). From the viewpoint of obtaining good curability, tetraalkoxytitanium is preferred, and tetraisopropoxytitanium is particularly preferred.

[0069] In terms of availability, compatibility with the organic polymer (A), and curability, tetraisopropoxytitanium, tetra tert-butoxytitanium, bis(acetylacetonato)diisopropoxytitanium, bis(ethylacetoacetate)diisobutoxytitanium, and bis(ethylacetoacetate)diisopropoxytitanium are more preferred, and bis(ethylacetoacetate)diisobutoxytitanium and bis(ethylacetoacetate)diisopropoxytitanium are particularly preferred. The titanium compound (b2) may be a single component or a combination of multiple components. The titanium compound (b2) may be a single component or a combination of multiple components. The titanium compound (b2) and the amidine compound (b1) may be added separately to the curable composition, or may be added to the curable composition as a mixture in which both are mixed in advance.

[0070] In terms of fast curing and low yellowing, the amount of titanium compound (b2) used is preferably 0.1 to 5.0 parts by weight, more preferably 0.5 to 4.5 parts by weight, and even more preferably 1.0 to 4.0 parts by weight, relative to 100 parts by weight of organic polymer (A). The weight ratio (b2) / (b1) of titanium compound (b2) to amidine compound (b1) is preferably 1.0 to 10, more preferably 1.0 to 5.0.

[0071] <Silane Condensate (C)> The silane condensate (C) is a compound having a structure represented by the following formula (4).

[0072] In formula (4), R 6 is a methyl group or an ethyl group. 6 may be the same or different. 7 , R 8 R is a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent. 7 , R 8 may be the same or different, and e and f are integers of 1 to 50.

[0073] The silane condensate (C) can be obtained by condensing a silane compound monomer having a hydrolyzable silicon group, followed by oligomerization or polymerization. Specific examples of the silane compound monomer that forms the silane condensate (C) include vinyltrialkoxysilanes such as vinyltrimethoxysilane and vinyltriethoxysilane; allyltrialkoxysilanes such as allyltrimethoxysilane and allyltriethoxysilane; γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropyltriethoxysilane, γ-(2- ... N-ethyl)aminoethyl)aminopropyltrimethoxysilane, γ-(6-aminohexyl)aminopropyltrimethoxysilane, 3-(N-ethylamino)-2-methylpropyltrimethoxysilane, γ-ureidopropyltrimethoxysilane, γ-ureidopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-benzyl-γ-aminopropyltrimethoxysilane, N-vinylbenzyl-γ-aminopropyltriethoxysilane, N-cyclohexylaminomethyltrimethoxysilane amino group-containing trialkoxysilanes such as i-thoxysilane, N-phenylaminomethyltrimethoxysilane, N-butylaminopropyltrimethoxysilane, and (2-aminoethyl)aminomethyltrimethoxysilane; alkyltrialkoxysilanes such as methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, isopropyltrimethoxysilane, and isopropyltriethoxysilane; cycloalkyltrialkoxysilanes such as cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, cycloheptyltrimethoxysilane, cycloheptyltriethoxysilane, 2-methylcyclohexyltrimethoxysilane, 2-methylcyclohexyltriethoxysilane, 3-methylcyclohexyltrimethoxysilane, 3-methylcyclohexyltriethoxysilane, 4-methylcyclohexyltrimethoxysilane, and 4-methylcyclohexyltriethoxysilane;Examples of suitable silane condensates include aryltrialkoxysilanes such as phenyltrimethoxysilane, phenyltriethoxysilane, 1-naphthyltrimethoxysilane, and 1-naphthyltriethoxysilane; and aralkyltrialkoxysilanes such as benzyltrimethoxysilane, benzyltriethoxysilane, phenethyltrimethoxysilane, and phenethyltriethoxysilane. Among these, it is preferable to form the silane condensate (C) using at least one trialkoxysilane selected from vinyltrialkoxysilane, amino group-containing trialkoxysilane, and alkyltrialkoxysilane, and it is more preferable to form the silane condensate (C) using at least one trimethoxysilane selected from vinyltrimethoxysilane, amino group-containing trimethoxysilane, and alkyltrimethoxysilane.

[0074] Specific examples of the silane condensate (C) include Dynasylan 6490, Dynasylan 6498, and Dynasylan 1146 manufactured by Evonik.

[0075] When the silane condensate (C) is added to the curable composition, the curable composition cures faster than when a silane compound monomer is added to the curable composition.

[0076] From the viewpoint of rapid curing, the amount of the silane condensate (C) used is preferably 0.1 to 20 parts by weight, more preferably 0.3 to 15 parts by weight, and even more preferably 0.5 to 10 parts by weight, relative to 100 parts by weight of the organic polymer (A). The curable composition may contain, together with the silane condensate (C), a silane coupling agent (silane compound) used as an adhesion promoter, physical property adjuster, dehydrating agent, etc., as described below. The silane coupling agent typically corresponds to the above-mentioned silane compound monomer. When the curable composition contains a silane coupling agent, the amount of the silane condensate (C) used is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, even more preferably 50% by mass or more, and particularly preferably 70% by mass or less, relative to the total mass of the silane condensate (C) and the silane coupling agent. From the viewpoint of rapid curing alone, it is preferable that the curable composition does not contain a silane coupling agent.

[0077] <Other Additives> The curable composition may contain other additives in addition to the organic polymer (A), the curing catalyst (B), and the silane condensate (C), as long as the desired effects are not impaired. Examples of other additives include silanol condensation catalysts other than the curing catalyst (B), fillers, adhesion promoters, plasticizers, solvents, diluents, thixotropy-imparting agents, antioxidants, light stabilizers, ultraviolet absorbers, physical property adjusters, tackifying resins, compounds containing epoxy groups, photocurable substances, oxygen-curable substances, epoxy resins, other resins, surface property improvers, foaming agents, curability adjusters, flame retardants, silicates, radical inhibitors, metal deactivators, phosphorus-based peroxide decomposers, lubricants, pigments, and mildew inhibitors.

[0078] (Silanol Condensation Catalyst) The curable composition may contain a silanol condensation catalyst other than the curing catalyst (B) described above, for the purpose of promoting the hydrolysis condensation reaction between reactive silicon groups in the organic polymer (A) and chain-extending or crosslinking the polymer. Examples of silanol condensation catalysts include organotin compounds, metal carboxylates, amine compounds, carboxylic acids, metal alkoxides, and inorganic acids. Two or more different silanol condensation catalysts may be used in combination. The amount of the silanol condensation catalyst used is preferably 0.001 to 20 parts by weight, more preferably 0.01 to 15 parts by weight, and particularly preferably 0.01 to 10 parts by weight, per 100 parts by weight of the organic polymer (A).

[0079] (Filler) The curable composition may contain various fillers. Examples of fillers include reinforcing fillers such as fumed silica, precipitated silica, crystalline silica, fused silica, dolomite, anhydrous silicic acid, hydrous silicic acid, and carbon black; heavy calcium carbonate, colloidal calcium carbonate, magnesium carbonate, diatomaceous earth, calcined clay, clay, talc, titanium oxide, bentonite, organic bentonite, ferric oxide, fine aluminum powder, flint powder, zinc oxide, activated zinc oxide, and resin powder; and fibrous fillers such as asbestos, glass fiber, and filaments. Examples of resin powders include PVC powder and PMMA powder. When a filler is used, the amount of filler used is preferably 1 to 300 parts by weight, more preferably 10 to 200 parts by weight, per 100 parts by weight of the organic polymer (A).

[0080] When a high-strength cured product is desired by using these fillers, fillers selected from the group consisting of fumed silica, precipitated silica, crystalline silica, fused silica, dolomite, silicic acid anhydride, hydrated silicic acid, carbon black, surface-treated fine calcium carbonate, calcined clay, clay, and activated zinc oxide are preferably used. The amount used is preferably 1 to 200 parts by weight per 100 parts by weight of the organic polymer (A). Furthermore, when a low-strength cured product with a high elongation at break is desired, preferable results can be obtained by using a filler selected from the group consisting of titanium oxide, calcium carbonate, magnesium carbonate, talc, ferric oxide, zinc oxide, and shirasu balloons in an amount ranging from 5 to 200 parts by weight per 100 parts by weight of the organic polymer (A).

[0081] The curable composition may contain spherical hollow bodies such as balloons to reduce the weight (specific gravity) of the cured product. Balloons are spherical fillers with hollow interiors. Examples of balloon materials include inorganic materials such as glass, shirasu, and silica, and organic materials such as phenolic resin, urea resin, polystyrene, saran, and acrylonitrile. The balloon material is not limited to these materials. The balloon material may also be a composite material composed of an inorganic material and an organic material. The balloon material may also be a laminate of multiple layers. One type of balloon may be used alone, or two or more types may be used in combination. The balloon surface may be surface-treated, coated, or treated with various surface treatment agents. For example, organic balloons coated with calcium carbonate, talc, titanium oxide, etc., or inorganic balloons surface-treated with a silane coupling agent may be used.

[0082] The particle size of the balloons is preferably 3 to 200 μm, and particularly preferably 10 to 110 μm. When the particle size of the balloons is within this range, the use of an appropriate amount of balloons can reduce the weight of the cured product to a desired extent, and a cured product can be formed while suppressing the occurrence of surface irregularities and a decrease in elongation.

[0083] The amount of spherical hollow bodies (balloons) used is preferably 0.01 to 30 parts by weight per 100 parts by weight of the organic polymer (A). The lower limit is more preferably 0.1 part by weight, and the upper limit is more preferably 20 parts by weight. Using spherical hollow bodies in an amount within the above range can improve workability while maintaining the elongation and breaking strength of the cured product.

[0084] (Adhesion Imparting Agent) The curable composition may contain an adhesion imparting agent. Examples of adhesion imparting agents include silane coupling agents that do not fall under the category of the silane condensate (C) described above. The silane coupling agent is a compound having a hydrolyzable silicon group and a functional group other than the hydrolyzable silicon group in the molecule. By using a silane coupling agent, when the curable composition is applied to various adherends, such as inorganic substrates such as glass, aluminum, stainless steel, zinc, copper, and mortar, or organic substrates such as vinyl chloride, acrylic, polyester, polyethylene, polypropylene, and polycarbonate, a significant adhesive improvement effect is exhibited under non-primer conditions or primer-treated conditions. When the curable composition is used under non-primer conditions, the effect of improving adhesion to various adherends is particularly significant. In addition to the above functions, the silane coupling agent can also function as a dehydrating agent, a physical property adjuster, a dispersibility improver for inorganic fillers, etc.

[0085] The hydrolyzable group in the hydrolyzable silicon group contained in the silane coupling agent is not particularly limited. Examples of hydrolyzable groups include hydrogen atoms, halogen atoms, alkoxy groups, aryloxy groups, alkenyloxy groups, acyloxy groups, ketoximate groups, amino groups, amide groups, acid amide groups, aminooxy groups, and mercapto groups. Among these, halogen atoms, alkoxy groups, alkenyloxy groups, and aryloxy groups are preferred because of their high activity. Chlorine atoms and alkoxy groups are preferred because they are easily introduced into the silane coupling agent. Alkoxy groups such as methoxy groups and ethoxy groups are more preferred because of their mild hydrolysis and ease of handling, with methoxy groups and ethoxy groups being particularly preferred. Furthermore, ethoxy groups and isopropenyloxy groups are preferred in terms of safety because the compounds that are eliminated by reaction are ethanol and acetone, respectively. The number of hydrolyzable groups bonded to the silicon atom in the silane coupling agent may be preferably three to ensure good adhesion. Furthermore, two may be preferable to ensure the storage stability of the curable composition.

[0086] When a silane coupling agent is used as an adhesion promoter, an aminosilane coupling agent having a hydrolyzable silicon group and a substituted or unsubstituted amino group is preferred because it has a significant effect of improving adhesion. The substituent in the substituted amino group is not particularly limited. Examples of the substituent include an alkyl group, an aralkyl group, and an aryl group.

[0087] Specific examples of aminosilane coupling agents include γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltriisopropoxysilane, γ-aminopropylmethyldimethoxysilane, γ-aminopropylmethyldiethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropylmethyldimethoxysilane, γ-(2-aminoethyl)aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropylmethyldiethoxysilane, γ-(2-aminoethyl)aminopropyltriisopropoxysilane, γ-(2-(2-aminoethyl)aminoethyl)aminopropyltrimethoxysilane, γ-(6-aminohexyl)aminopropyltrimethoxysilane, and 3-(N-ethylamino)-2-methylpropyltrimethoxysilane. amino group-containing silanes such as γ-ureidopropyltrimethoxysilane, γ-ureidopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-benzyl-γ-aminopropyltrimethoxysilane, N-vinylbenzyl-γ-aminopropyltriethoxysilane, N-cyclohexylaminomethyltriethoxysilane, N-cyclohexylaminomethyldiethoxymethylsilane, N-phenylaminomethyltrimethoxysilane, N-butylaminopropyltrimethoxysilane, (2-aminoethyl)aminomethyltrimethoxysilane, N,N'-bis[3-(trimethoxysilyl)propyl]ethylenediamine, and bis(trimethoxysilylpropyl)amine; and ketimine-type silanes such as N-(1,3-dimethylbutylidene)-3-(triethoxysilyl)-1-propanamine.

[0088] Of these, γ-aminopropyltrimethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, and γ-(2-aminoethyl)aminopropylmethyldimethoxysilane are preferred in order to obtain good adhesion properties in the cured product. Only one type of aminosilane coupling agent may be used, or two or more types may be used in combination. γ-(2-aminoethyl)aminopropyltrimethoxysilane has been noted to be more irritating than other aminosilanes. The irritating properties can be alleviated by using γ-aminopropyltrimethoxysilane in combination with γ-(2-aminoethyl)aminopropyltrimethoxysilane instead of reducing the amount of γ-(2-aminoethyl)aminopropyltrimethoxysilane. γ-aminopropyltrimethoxysilane and γ-(2-aminoethyl)aminopropylmethyldimethoxysilane are preferred in order to ensure good storage stability of the curable composition.

[0089] Specific examples of silane coupling agents other than aminosilane coupling agents include epoxy group-containing silane coupling agents such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltriethoxysilane; isocyanate group-containing silane coupling agents such as γ-isocyanatepropyltrimethoxysilane, γ-isocyanatepropyltriethoxysilane, γ-isocyanatepropylmethyldiethoxysilane, γ-isocyanatepropylmethyldimethoxysilane, (isocyanatemethyl)trimethoxysilane, and (isocyanatemethyl)dimethoxymethylsilane; and γ-mercaptopropyltrimethoxysilane and γ-mercaptopropyltriethoxysilane. mercapto group-containing silane coupling agents such as γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropylmethyldiethoxysilane, and mercaptomethyltriethoxysilane; carboxy silane coupling agents such as β-carboxyethyltriethoxysilane, β-carboxyethylphenylbis(2-methoxyethoxy)silane, and N-β-(carboxymethyl)aminoethyl-γ-aminopropyltrimethoxysilane; vinyl-type unsaturated group-containing silane coupling agents such as vinyltrimethoxysilane, vinyltriethoxysilane, γ-methacryloyloxypropylmethyldimethoxysilane, and γ-acryloyloxypropylmethyltriethoxysilane; halogen-containing silane coupling agents such as γ-chloropropyltrimethoxysilane; and isocyanurate silane coupling agents such as tris(trimethoxysilyl)isocyanurate.

[0090] Of these, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, and γ-glycidoxypropylmethyldimethoxysilane are preferred in order to obtain good adhesive properties in the cured product.

[0091] The silane coupling agent may be used alone or in combination of two or more. The amount of the silane coupling agent used is not particularly limited as long as the desired effect is not impaired. The amount of the silane coupling agent used is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, per 100 parts by weight of the organic polymer (A).

[0092] (Plasticizer) The curable composition may contain a plasticizer. Addition of a plasticizer makes it possible to adjust the viscosity and slump of the curable composition, as well as the mechanical properties such as tensile strength and elongation of the cured product.

[0093] Specific examples of the plasticizer include phthalate ester compounds other than the phthalate ester (B), such as dibutyl phthalate, diisononyl phthalate (DINP), diheptyl phthalate, di(2-ethylhexyl) phthalate, diisodecyl phthalate (DIDP), and butyl benzyl phthalate; terephthalate ester compounds such as bis(2-ethylhexyl)-1,4-benzenedicarboxylate; non-phthalate ester compounds such as 1,2-cyclohexanedicarboxylic acid diisononyl ester; dioctyl adipate, dioctyl sebacate, and dibutyl sebacate. Examples of suitable terephthalic acid ester compounds include aliphatic polycarboxylic acid ester compounds such as diisodecyl succinate and tributyl acetyl citrate; unsaturated fatty acid ester compounds such as butyl oleate and methyl acetylricinoleate; alkylsulfonic acid phenyl esters; phosphate ester compounds such as tricresyl phosphate and tributyl phosphate; trimellitic acid ester compounds; chlorinated paraffins; hydrocarbon oils such as alkyldiphenyls and partially hydrogenated terphenyls; process oils; epoxidized soybean oil and epoxy plasticizers such as benzyl epoxy stearate. Specific examples of terephthalic acid ester compounds include EASTMAN 168 (trade name, manufactured by EASTMAN CHEMICAL). Specific examples of non-phthalic acid ester compounds include Hexamoll DINCH (trade name, manufactured by BASF). Specific examples of alkylsulfonic acid phenyl esters include Mesamoll (trade name, manufactured by LANXESS).

[0094] Polymeric plasticizers can also be used. The use of polymeric plasticizers allows the initial physical properties of the cured product to be maintained for a longer period of time than when low-molecular-weight plasticizers are used. Furthermore, the drying properties (paintability) of the cured product when coated with an alkyd paint are improved.

[0095] Specific examples of polymeric plasticizers include vinyl polymers, which are polymers of vinyl monomers; esters of polyalkylene glycols and polyols, such as diethylene glycol dibenzoate, triethylene glycol dibenzoate, and pentaerythritol ester; polyester plasticizers obtained from dibasic acids, such as sebacic acid, adipic acid, azelaic acid, and phthalic acid, and dihydric alcohols, such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, and dipropylene glycol; polyether polyols, such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol, having a number average molecular weight of 500 or more, or even 1,000 or more; derivatives in which the hydroxy groups of these polyether polyols have been converted to ester groups, ether groups, or the like; polystyrenes, such as poly-α-methylstyrene; polybutadiene, polybutene, polyisobutylene, butadiene-acrylonitrile, and polychloroprene. Polymeric plasticizers are not limited to these.

[0096] The polymeric plasticizer is preferably compatible with the organic polymer (A). From this viewpoint, polyethers and vinyl polymers are preferred. When polyethers are used as plasticizers, surface curing and deep curing properties are improved, and curing delay after storage does not occur. Among polyethers, polypropylene glycol is more preferred. Furthermore, vinyl polymers are preferred from the viewpoints of compatibility with the polymer (A) and the weather resistance and heat resistance of the cured product. Among vinyl polymers, acrylic polymers and / or methacrylic polymers are preferred, with acrylic polymers such as polyacrylic acid alkyl esters being more preferred. As a method for synthesizing vinyl polymers, living radical polymerization is preferred, and atom transfer radical polymerization is more preferred, since it produces polymers with narrow molecular weight distributions and low viscosity. Furthermore, the so-called SGO process, which is described in JP 2001-207157 A and which involves continuous bulk polymerization of acrylic acid alkyl ester monomers at high temperature and high pressure, is also preferred as a method for producing vinyl polymers.

[0097] The number-average molecular weight of the polymeric plasticizer is preferably 500 to 15,000, more preferably 800 to 10,000, even more preferably 1,000 to 8,000, particularly preferably 1,000 to 5,000, and most preferably 1,000 to 3,000. When the number-average molecular weight of the polymeric plasticizer is within the above range, the initial physical properties of the cured product can be maintained over a long period of time while suppressing the leaching of the plasticizer from the cured product over time due to heat, rain, etc., and the curable composition has an appropriate viscosity and good workability. The molecular weight distribution of the polymeric plasticizer is not particularly limited, but a narrow one is preferable. Specifically, the molecular weight distribution is preferably less than 1.80, more preferably 1.70 or less, even more preferably 1.60 or less, even more preferably 1.50 or less, particularly preferably 1.40 or less, and most preferably 1.30 or less.

[0098] The number average molecular weight of a vinyl polymer is measured by GPC. The number average molecular weight of a polyether polymer is measured by end group analysis. The molecular weight distribution (Mw / Mn) is measured by GPC (polystyrene equivalent).

[0099] The polymeric plasticizer may or may not have a reactive silicon group. When the polymeric plasticizer has a reactive silicon group, the polymeric plasticizer acts as a reactive plasticizer, preventing the plasticizer from migrating from the cured product. When the polymeric plasticizer has a reactive silicon group, the number of reactive silicon groups per molecule is preferably 1 or less on average, more preferably 0.8 or less. When using a plasticizer having a reactive silicon group, particularly a polyether polymer having a reactive silicon group, it is necessary that its number average molecular weight is lower than that of the organic polymer (A).

[0100] The amount of plasticizer used is preferably 5 to 150 parts by weight, more preferably 10 to 120 parts by weight, and even more preferably 20 to 100 parts by weight, per 100 parts by weight of the organic polymer (A). When the amount of plasticizer used is within the above range, it is possible to form a cured product having excellent mechanical strength while fully obtaining the desired effects of using the plasticizer. The plasticizer may be used alone or in combination of two or more types. A low-molecular-weight plasticizer and a polymeric plasticizer may be used in combination. These plasticizers may be blended with the organic polymer (A) when producing the polymer (A).

[0101] (Solvent, Diluent) The curable composition may contain a solvent or a diluent. The solvent and diluent are not particularly limited. Examples of solvents and diluents that can be used include aliphatic hydrocarbons, aromatic hydrocarbons, alicyclic hydrocarbons, halogenated hydrocarbons, alcohols, esters, ketones, and ethers. When using a solvent or a diluent, in view of the problem of air pollution when the curable composition is used indoors, the boiling point of the solvent is preferably 150°C or higher, more preferably 200°C or higher, and particularly preferably 250°C or higher. The above solvents or diluents may be used alone or in combination of two or more.

[0102] (Thixotropy-imparting agent) The curable composition may contain a thixotropy-imparting agent, if necessary, to prevent sagging and improve workability. The thixotropy-imparting agent is not particularly limited. Examples of thixotropy-imparting agents include polyamide waxes; hydrogenated castor oil derivatives; and metal soaps such as calcium stearate, aluminum stearate, and barium stearate. Examples of trade names include Disparlon 6500, Disparlon 308, Disparlon 6300, Crayvallac SL, and Crayvallac SLT. These thixotropy-imparting agents may be used alone or in combination of two or more. The amount of the thixotropy-imparting agent used is preferably 0.1 to 20 parts by weight per 100 parts by weight of the polymer (A).

[0103] (Antioxidant) The curable composition may contain an antioxidant (antiaging agent). Use of an antioxidant can improve the weather resistance of the cured product. Examples of antioxidants include hindered phenol compounds, monophenol compounds, bisphenol compounds, and polyphenol compounds, with hindered phenols being particularly preferred. Examples of antioxidants include Irganox 245, Irganox 1010, Irganox 1035, Irganox 1076, Irganox 1135, Irganox 1330, and Irganox 1520 (all manufactured by BASF); SONGNOX 1076 (manufactured by SONGWON), and BHT. Hindered amine light stabilizers such as TINUVIN 622LD, TINUVIN 144, TINUVIN 292, CHIMASSORB 944LD, and CHIMASSORB 119FL (all manufactured by BASF); Adeka STAB LA-57, Adeka STAB LA-62, Adeka STAB LA-67, Adeka STAB LA-63, and Adeka STAB LA-68 (all manufactured by ADEKA Corporation); Sanol LS-2626, Sanol LS-1114, and Sanol LS-744 (all manufactured by Sankyo Lifetech Co., Ltd.); and Nocrac CD (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) can also be used. Additionally, antioxidants such as SONGNOX 4120, Nauguard 445, and OKABEST CLX050 can also be used. Specific examples of antioxidants are also described in JP-A Nos. 4-283259 and 9-194731. The amount of antioxidant used is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, per 100 parts by weight of polymer (A).

[0104] (Light Stabilizer) The curable composition may contain a light stabilizer. Use of a light stabilizer can prevent photooxidative degradation of the cured product. Examples of light stabilizers include benzotriazole compounds, hindered amine compounds, and benzoate compounds. As the light stabilizer, hindered amine compounds are particularly preferred. The amount of the light stabilizer used is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, per 100 parts by weight of the polymer (A). Specific examples of light stabilizers are described in, for example, JP-A-9-194731.

[0105] When a photocurable substance is blended into the curable composition, particularly when an unsaturated acrylic compound is used, it is preferable to use a tertiary amine-containing hindered amine light stabilizer as the hindered amine light stabilizer, as described in JP-A-5-70531, in order to improve the storage stability of the curable composition. Examples of tertiary amine-containing hindered amine light stabilizers include TINUVIN 123, TINUVIN 144, TINUVIN 249, TINUVIN 292, TINUVIN 312, TINUVIN 622LD, TINUVIN 765, TINUVIN 770, TINUVIN 880, TINUVIN 5866, TINUVIN B97, CHIMASSORB 119FL, and CHIMASSORB 944LD (all manufactured by BASF); Adekastab LA-57, LA-62, LA-63, LA-67, and LA-68 (all manufactured by ADEKA Corporation); Sanol LS-292, LS-2626, LS-765, LS-744, and LS-1114 (all manufactured by Sankyo Lifetech Co., Ltd.), SABOSTAB UV91, SABOSTAB Examples include UV119, SONGSORB CS5100, SONGSORB CS622, SONGSORB CS944 (all manufactured by SONGWON), and Nocrac CD (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.).

[0106] (UV absorber) The curable composition may contain a UV absorber. Use of a UV absorber can improve the surface weather resistance of the cured product. Examples of UV absorbers include benzophenone-based compounds, benzotriazole-based compounds, salicylate-based compounds, triazine-based compounds, substituted tolyl-based compounds, and metal chelate-based compounds. Among these, benzotriazole-based compounds are particularly preferred. Specific examples of benzotriazole-based compounds include TINUVIN 234, TINUVIN 326, TINUVIN 327, TINUVIN 328, TINUVIN 329, TINUVIN 350, TINUVIN 571, TINUVIN 900, TINUVIN 928, TINUVIN 1130, and TINUVIN 1600 (all manufactured by BASF); and SONGSORB 3290 (manufactured by SONGWON). Specific examples of triazine-based compounds include TINUVIN 400, TINUVIN 405, TINUVIN 477, and TINUVIN 1577ED (all manufactured by BASF); SONGSORB CS400 and SONGSORB 1577 (manufactured by SONGWON). Specific examples of benzophenone-based compounds include SONGSORB 8100 (manufactured by SONGWON). The amount of UV absorber used is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, per 100 parts by weight of polymer (A). It is preferable to use a phenol-based antioxidant or hindered phenol-based antioxidant in combination with a hindered amine-based light stabilizer and a benzotriazole-based UV absorber. Addworks IBC 760 (manufactured by Clariant) can be used as a mixture of an antioxidant, a light stabilizer, and a UV absorber.

[0107] (Physical Property Adjuster) The curable composition may contain a physical property adjuster to adjust the tensile properties of the cured product, as necessary. The physical property adjuster is not particularly limited. Examples of the physical property adjuster include alkylalkoxysilanes such as methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, and n-propyltrimethoxysilane; alkylisopropenoxysilanes such as dimethyldiisopropenoxysilane, methyltriisopropenoxysilane, and γ-glycidoxypropylmethyldiisopropenoxysilane; alkoxysilanes having a functional group such as γ-glycidoxypropylmethyldimethoxysilane, γ-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, vinyldimethylmethoxysilane, γ-aminopropyltrimethoxysilane, N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane, γ-mercaptopropyltrimethoxysilane, and γ-mercaptopropylmethyldimethoxysilane; silicone varnishes; and polysiloxanes. The use of a physical property modifier can increase the hardness of the cured product, or conversely, decrease the hardness of the cured product and increase the elongation at break. The physical property modifiers may be used alone or in combination of two or more.

[0108] In particular, compounds that hydrolyze to form a compound having a monovalent silanol group in the molecule have the effect of reducing the modulus of the cured product without increasing the stickiness of the surface of the cured product. Compounds that hydrolyze to form a compound having a monovalent silanol group in the molecule are particularly preferred, with compounds that form trimethylsilanol being particularly preferred. Examples of compounds that hydrolyze to form a compound having a monovalent silanol group in the molecule include the compounds described in JP-A-5-117521. Other examples include derivatives of alkyl alcohols such as hexanol, octanol, and decanol that hydrolyze to form trialkylsilanols such as trimethylsilanol, and derivatives of polyhydric alcohols having three or more hydroxyl groups such as trimethylolpropane, glycerin, pentaerythritol, or sorbitol that hydrolyze to form trialkylsilanols such as trimethylsilanol, as described in JP-A-11-241029. Examples include derivatives of oxyalkylene polymers that produce silicon compounds that produce trialkylsilanols such as trimethylsilanol upon hydrolysis, as described in JP-A-7-258534. Furthermore, polymers having crosslinkable hydrolyzable silicon-containing groups and silicon-containing groups that can be hydrolyzed to monosilanol-containing compounds, as described in JP-A-6-279693, can also be used. The physical property adjuster is used in an amount of 0.1 to 20 parts by weight, preferably 0.5 to 10 parts by weight, per 100 parts by weight of polymer (A).

[0109] (Tackifying Resin) The curable composition may contain a tackifying resin for purposes such as enhancing the adhesion and cohesion of the cured product to a substrate. The tackifying resin is not particularly limited, and tackifying resins commonly used in various curable compositions can be used. Specific examples of tackifying resins include terpene resins, aromatic modified terpene resins, hydrogenated terpene resins, terpene-phenol resins, phenol resins, modified phenol resins, xylene-phenol resins, cyclopentadiene-phenol resins, coumarone-indene resins, rosin resins, rosin ester resins, hydrogenated rosin ester resins, xylene resins, low-molecular-weight polystyrene resins, styrene copolymer resins, styrene block copolymers, hydrogenated styrene block copolymers, petroleum resins, hydrogenated petroleum resins, and DCPD resins. Examples of petroleum resins include C5 hydrocarbon resins, C9 hydrocarbon resins, and C5C9 hydrocarbon copolymer resins. These may be used alone or in combination of two or more. The amount of the tackifier resin used is preferably 2 to 100 parts by weight, more preferably 5 to 50 parts by weight, and even more preferably 5 to 30 parts by weight, per 100 parts by weight of the polymer (A). Using an amount of the tackifier resin within this range allows for the formation of a cured product with good adhesion and cohesion to the substrate. The curable composition has an appropriate viscosity, and the handleability of the curable composition is good.

[0110] (Epoxy Group-Containing Compound) The curable composition may contain a compound containing an epoxy group. Use of a compound containing an epoxy group can improve the recovery of the cured product. Examples of compounds containing an epoxy group include epoxidized unsaturated fats and oils, epoxidized unsaturated fatty acid esters, alicyclic epoxy compounds, epichlorohydrin derivatives, and mixtures thereof. Specific examples of compounds containing an epoxy group include epoxidized soybean oil, epoxidized linseed oil, bis(2-ethylhexyl)-4,5-epoxycyclohexane-1,2-dicarboxylate (E-PS), epoxy octyl stearate, and epoxy butyl stearate. The amount of the epoxy group-containing compound used is preferably 0.5 to 50 parts by weight per 100 parts by weight of polymer (A).

[0111] (Epoxy Resin) The curable composition may contain an epoxy resin. Curable compositions containing an epoxy resin are preferred as adhesives, particularly adhesives for exterior wall tiles. Examples of epoxy resins include bisphenol A-type epoxy resins and novolac-type epoxy resins. The weight ratio of the polymer (A) to the epoxy resin is preferably in the range of 100 / 1 to 1 / 100, expressed as (weight of polymer (A)) / (weight of epoxy resin). When the polymer (A) and the epoxy resin are used in the above ratio, a high-strength cured product with excellent impact strength and toughness is easily formed. When an epoxy resin is used, the curable composition may contain a curing agent together with the epoxy resin. The type of curing agent is not particularly limited, and commonly used curing agents can be used. The amount of curing agent used is preferably 0.1 to 300 parts by weight per 100 parts by weight of the epoxy resin.

[0112] (Photocurable Substance) The curable composition may contain a photocurable substance. The use of a photocurable substance forms a coating of the photocurable substance on the surface of the cured product, improving the stickiness and weather resistance of the cured product. Various compounds, such as organic monomers, oligomers, and resins, are known as photocurable substances. Many compositions containing photocurable substances are also known. Representative photocurable substances include unsaturated acrylic compounds, polyvinyl cinnamates, and azido resins. Examples of unsaturated acrylic compounds include monomers, oligomers, or mixtures thereof having one or more acrylic or methacrylic unsaturated groups. The amount of photocurable substance used is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, per 100 parts by weight of polymer (A). Using a photocurable substance in this range facilitates the formation of a flexible cured product with excellent weather resistance and reduced cracking.

[0113] (Oxygen-Curable Substance) The curable composition may contain an oxygen-curable substance. Examples of oxygen-curable substances include unsaturated compounds that can react with oxygen in the air. When the curable substance contains an oxygen-curable substance, the oxygen-curable substance reacts with oxygen in the air to form a cured film near the surface of the cured product. The formation of a cured film on the surface of the cured product can prevent stickiness and the adhesion of dirt and dust to the surface of the cured product. Specific examples of oxygen-curable substances include drying oils such as tung oil and linseed oil; various alkyd resins obtained by modifying drying oils; acrylic polymers, epoxy resins, and silicone resins modified with drying oils; and liquid polymers such as 1,2-polybutadiene, 1,4-polybutadiene, or polymers of C5 to C8 dienes obtained by polymerizing or copolymerizing diene compounds such as butadiene, chloroprene, isoprene, or 1,3-pentadiene. These may be used alone or in combination of two or more types. The amount of oxygen-curable substance used is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, per 100 parts by weight of polymer (A). Using an amount of oxygen-curable substance within this range makes it easier to form a cured product whose surface is less susceptible to contamination by dirt and dust and has excellent mechanical properties such as tensile strength. As described in JP-A-3-160053, the oxygen-curable substance is preferably used in combination with a photo-curable substance.

[0114] <Preparation of Curable Composition> The curable composition can be prepared as a one-component composition by mixing all ingredients in advance, sealing, and storing them, and then curing them with moisture in the air after application. A one-component curable composition can be prepared by mixing the organic polymer (A), the condensation catalyst (B), and the silane condensate (C) with the optional ingredients described above, as needed. The curing agent composition can also be prepared as a two-component composition by mixing a curing agent containing the curing catalyst (B), the silane condensate (C), and ingredients such as a filler, plasticizer, and water with a separately prepared composition containing the organic polymer (A) before use. From the standpoint of workability, the one-component composition is preferred. In preparing the curable composition, it is preferable to previously mix the silane condensate (C) obtained by condensing the silane compound monomer described above with the other ingredients, rather than producing the silane condensate (C) by mixing the silane compound monomer described above with the other ingredients and then condensing. When the curable composition is a one-component type, all of the components are blended in advance, and therefore, it is preferable that the components containing water are dehydrated and dried before use, or dehydrated under reduced pressure during blending and kneading. In addition to the dehydration and drying method, the storage stability can be further improved by adding an alkoxysilane compound such as methyltrimethoxysilane, phenyltrimethoxysilane, n-propyltrimethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropylmethyldiethoxysilane, or γ-glycidoxypropyltrimethoxysilane. The amount of the dehydrating agent, particularly a silicon compound capable of reacting with water such as vinyltrimethoxysilane, used is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, per 100 parts by weight of polymer (A).

[0115] The curable composition can be used as a construction sealant, industrial adhesive, waterproof coating film-forming composition, pressure-sensitive adhesive raw material, and the like. The curable composition can also be used as a sealant for buildings, ships, automobiles, roads, and the like. Furthermore, the curable composition can adhere to a wide range of substrates, such as glass, porcelain, wood, metal, and resin moldings, either alone or with the aid of a primer. Therefore, the curable composition can also be used as various types of sealing compositions and adhesive compositions. In addition to conventional adhesives, the curable composition can also be used as a contact adhesive. Furthermore, the curable composition is useful as a food packaging material, a cast rubber material, a molding material, and a paint. The cured product of the above curable composition exhibits low water absorption. Therefore, the above curable composition and its cured product are particularly suitable for waterproof materials such as sealants, waterproof adhesives, and waterproof coatings.

[0116] <Method for Producing a Cured Product> Before curing, the curable composition is formed into a desired shape by a method such as coating, casting, or filling.

[0117] The curable composition that has been applied, cast, or filled and shaped is cured under a desired environment, such as room temperature and humidity.

[0118] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.

[0119] That is, one aspect of the present invention includes the following: <1> A curable composition comprising an organic polymer (A), a curing catalyst (B), and a silane condensate (C), wherein the organic polymer (A) is a compound represented by the following formula (1): -SiR 1 X 2 (1) (In formula (1), R 1is a hydrocarbon group having 1 to 20 carbon atoms, and X is a hydroxyl group or a hydrolyzable group, and two Xs may be the same or different. The curing catalyst (B) contains an amidine compound (b1) and a titanium compound (b2), and the amidine compound (b1) is a compound represented by the following formula (2): R 2 N=CR 3 -NR 4 2 (2) (In formula (2), R 2 , R 3 , and R 4 is a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, and two R 4 may be the same or different, and R 2 , R 3 , and two R 4 any two of these may be bonded to form a ring, and the titanium compound (b2) is a compound represented by the following formula (3): Ti(OR 5 ) d Y 4-d (3) (In formula (3), R 5 is a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, Y is a chelate coordination compound, and d is an integer of 0 to 4, or a condensate thereof, and the silane condensate (C) is a compound represented by the following formula (4): (In formula (4), R 6 is a methyl group or an ethyl group, and R 6 may be the same or different, R 7 , R 8 is a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, and R 7 , R 8 may be the same or different, and e and f are integers of 1 to 50. <2> A curable composition comprising a compound represented by the formula: 6is a methyl group. <3> The curable composition according to <1> or <2>, wherein the silane condensate (C) is a condensate of at least one trimethoxysilane selected from vinyltrimethoxysilane, amino group-containing trimethoxysilane, and alkyltrimethoxysilane. <4> The curable composition according to any one of <1> to <3>, wherein d in formula (3) represents 0 or an integer of 1 to 3. <5> The curable composition according to any one of <1> to <4>, wherein the main chain structure of the organic polymer (A) is polyoxyalkylene. <6> The curable composition according to any one of <1> to <5>, wherein the amidine compound (b1) is DBU (1,8-diazabicyclo[5.4.0]-7-undecene). <7> The curable composition according to any one of <1> to <6>, wherein the weight ratio (b2) / (b1) of the titanium compound (b2) to the amidine compound (b1) is 1.0 to 10.

[0120] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0121] <Preparation Example of Organic Polymer (A)> Hereinafter, the number average molecular weight is a GPC molecular weight measured under the following conditions: Solution delivery system: HLC-8120GPC manufactured by Tosoh Corporation Column: TSK-GEL H type manufactured by Tosoh Corporation Solvent: THF Molecular weight: Polystyrene equivalent Measurement temperature: 40°C

[0122] The end group-based molecular weight in the examples is a molecular weight calculated by determining the hydroxyl value according to the measurement method of JIS K 1557 and the iodine value according to the measurement method of JIS K 0070, taking into consideration the structure of the organic polymer. The structure of the organic polymer taken into consideration is the degree of branching, which is determined by the polymerization initiator used.

[0123] The average number of reactive silicon groups per terminal of the organic polymer shown in the examples is 1 H-NMR (using a Bruker AVANCE III HD-500) 3 The values ​​were calculated based on measurements using a fluorine-containing solvent.

[0124] (Preparation Example 1: Organic Polymer (A-1)) Using a 1 / 1 (weight ratio) mixture of polyoxypropylene diol having a molecular weight of approximately 2,000 and polyoxypropylene triol having a molecular weight of 3,000 as an initiator, propylene oxide was polymerized in the presence of a zinc hexacyanocobaltate glyme complex catalyst to obtain hydroxyl-terminated polypropylene oxide having a number average molecular weight of 19,000.

[0125] A methanol solution of 1.2 molar equivalents of NaOMe was added to the hydroxyl groups of the resulting hydroxyl-terminated polyoxypropylene. After distilling off the methanol from the reaction solution, allyl chloride was further added to the reaction solution to convert the terminal hydroxyl groups to allyl groups. Unreacted allyl chloride was removed by devolatilization under reduced pressure. As a result, polypropylene oxide having an allyl terminal and a number average molecular weight of approximately 19,000 was obtained. 100 parts by weight of the resulting unpurified allyl-terminated polyoxypropylene was mixed with 300 parts by weight of n-hexane and 300 parts by weight of water and stirred. The mixture was then separated into an aqueous phase and a hexane phase by centrifugation, and the aqueous phase was removed. The resulting hexane phase was again mixed with 300 parts by weight of water and stirred. The mixture was then separated into an aqueous phase and a hexane phase by centrifugation, and the aqueous phase was removed. The hexane was then removed from the recovered hexane phase by devolatilization under reduced pressure. In this manner, purified allyl-terminated polypropylene oxide (hereinafter referred to as allyl polymer) was obtained.

[0126] To 100 parts by weight of the resulting allyl polymer, 150 ppm of an isopropanol solution of platinum vinyldisiloxane complex with a platinum content of 3 wt % was added as a catalyst. Next, 0.7 molar equivalents of dimethoxymethylsilane were added relative to the allyl groups of the allyl polymer, and the allyl group terminals and dimethoxymethylsilane were reacted at 90°C for 5 hours to obtain dimethoxymethylsilyl-terminated polypropylene oxide (A-1). The number of dimethoxymethylsilyl groups per polymer chain terminal was approximately 0.7.

[0127] Preparation Example 2: Organic Polymer (A-2) Using a polyoxypropylene diol having a molecular weight of approximately 2,000 as an initiator, propylene oxide was polymerized in the presence of a zinc hexacyanocobaltate glyme complex catalyst to obtain hydroxyl-terminated polypropylene oxide having a number average molecular weight of 28,500.

[0128] Relative to the hydroxyl groups of the obtained hydroxyl-terminated polypropylene oxide, 1.0 molar equivalent of a methanol solution of NaOMe was added. After distilling off methanol from the reaction solution at 140°C, an additional 1.0 molar equivalent of allyl glycidyl ether was added to the reaction solution and reacted for 2 hours. Allyl chloride was then added to convert the terminal hydroxyl groups to allyl groups. As a result, an allyl polymer having a number average molecular weight of approximately 28,500 and multiple terminal allyl groups was obtained. The allyl polymer was purified using the same procedure as in Preparation Example 1. To 100 parts by weight of the obtained allyl polymer, 150 ppm of an isopropanol solution of a platinum vinyldisiloxane complex containing 3 wt% platinum was added as a catalyst. Next, 0.8 molar equivalent of dimethoxymethylsilane relative to the allyl groups of the allyl polymer was added, and the allyl terminals and dimethoxymethylsilane were reacted at 90°C for 5 hours to obtain dimethoxymethylsilyl-terminated polypropylene oxide (A-2). The number of dimethoxymethylsilyl groups per polymer chain end was about 1.5.

[0129] Preparation Example 3: Organic Polymer (A-3) Using polyoxypropylene triol having a molecular weight of approximately 3,000 as an initiator, propylene oxide was polymerized in the presence of a zinc hexacyanocobaltate glyme complex catalyst to obtain hydroxyl-terminated polypropylene oxide having a branched structure in the main chain and a number average molecular weight of approximately 25,000.

[0130] The allyl polymer was purified using the same procedures as in Preparation Example 1. To 100 parts by weight of the obtained allyl polymer, 150 ppm of an isopropanol solution of platinum vinyldisiloxane complex with a platinum content of 3 wt % was added as a catalyst. Next, 0.7 molar equivalents of dimethoxymethylsilane relative to the allyl groups of the allyl polymer were added, and the allyl group terminals and dimethoxymethylsilane were reacted at 90°C for 5 hours to obtain dimethoxymethylsilyl-terminated polypropylene oxide (A-3). The number of dimethoxymethylsilyl groups per polymer chain terminal was approximately 0.7.

[0131] Preparation Example 4: Organic Polymer (A-4) Using polyoxypropylene triol having a molecular weight of approximately 4,500 as an initiator, propylene oxide was polymerized in the presence of a zinc hexacyanocobaltate glyme complex catalyst to obtain hydroxyl-terminated polypropylene oxide having a number average molecular weight of approximately 14,300.

[0132] A methanol solution of 1.2 molar equivalents of NaOMe was added to the hydroxyl groups of the resulting hydroxyl-terminated polypropylene oxide. After distilling off the methanol from the reaction solution, allyl chloride was further added to the reaction solution to convert the terminal hydroxyl groups to allyl groups. This resulted in an allyl polymer with a number-average molecular weight of approximately 14,300 and terminated with allyl groups. The allyl polymer was purified using the same procedures as in Preparation Example 1. To 100 parts by weight of the resulting allyl polymer, 150 ppm of an isopropanol solution of platinum vinyldisiloxane complex containing 3 wt% platinum was added as a catalyst. Next, 0.8 molar equivalents of dimethoxymethylsilane were added to the allyl groups of the allyl polymer, and the allyl terminals and dimethoxymethylsilane were reacted at 90°C for 5 hours to yield dimethoxymethylsilyl-terminated polypropylene oxide (A-4). The number of dimethoxymethylsilyl groups per polymer chain end was approximately 0.8.

[0133] Preparation Example 5: Organic Polymer (A-5) 22 parts by weight of isobutyl alcohol was placed in a four-neck flask equipped with a stirrer, and the temperature was raised to 90°C under a nitrogen atmosphere. A mixed solution prepared by dissolving 14.8 parts by weight of methyl methacrylate, 60.6 parts by weight of butyl acrylate, 20.1 parts by weight of stearyl methacrylate, 4.5 parts by weight of 3-(dimethoxymethylsilyl)propyl methacrylate, and 1.9 parts by weight of 2,2'-azobis(2-methylbutyronitrile) in 17.1 parts by weight of isobutyl alcohol was added dropwise to the flask over 5 hours. Further, a mixed solution prepared by dissolving 0.2 parts by weight of 2,2'-azobis(2-methylbutyronitrile) in 1.8 parts by weight of isobutyl alcohol was added, and a polymerization reaction was carried out at 90°C for 2 hours. As a result of the above, an isobutyl alcohol solution (solid content 70% by weight) of poly(meth)acrylate (a-1) having an average of 1.8 dimethoxymethylsilyl groups per molecule and a number average molecular weight of 9,800 was obtained.

[0134] 70 parts by weight of the organic polymer (A-4) obtained in Preparation Example 4 and 42.8 parts by weight of an isobutyl alcohol solution of the organic polymer (a-1) were mixed, and the isobutyl alcohol was removed by devolatilization under reduced pressure. As a result, a polymer mixture (A-5) having a weight ratio of the organic polymer (A-4) / the organic polymer (a-1) of 70 / 30 was obtained.

[0135] Preparation Example 6: Organic Polymer (A-6) Using a polyoxypropylene diol having a molecular weight of approximately 2,000 as an initiator, propylene oxide was polymerized in the presence of a zinc hexacyanocobaltate glyme complex catalyst to obtain hydroxyl-terminated polypropylene oxide having a number average molecular weight of approximately 16,000.

[0136] A methanol solution of 1.2 molar equivalents of NaOMe was added to the hydroxyl groups of the resulting hydroxyl-terminated polypropylene oxide. After distilling off the methanol from the reaction solution, allyl chloride was further added to the reaction solution to convert the terminal hydroxyl groups to allyl groups. This resulted in an allyl polymer with a number-average molecular weight of approximately 14,300 and terminated with allyl groups. The allyl polymer was purified using the same procedures as in Preparation Example 1. To 100 parts by weight of the resulting allyl polymer, 150 ppm of an isopropanol solution of platinum vinyldisiloxane complex containing 3 wt% platinum was added as a catalyst. Next, 0.6 molar equivalents of dimethoxymethylsilane were added to the allyl groups of the allyl polymer, and the allyl terminals and dimethoxymethylsilane were reacted at 90°C for 5 hours to yield dimethoxymethylsilyl-terminated polypropylene oxide (A-6). The number of dimethoxymethylsilyl groups per polymer chain end was approximately 0.6.

[0137] <Synthesis Examples of Curing Catalyst (B)> (Synthesis Example 1: Composite 1) 30 g of TC-750 (bis(ethylacetoacetate)diisopropoxytitanium, manufactured by Matsumoto Fine Chemical Co., Ltd.) was added to a 200 mL recovery flask. While stirring the contents of the flask, 10 g of DBU (1,8-diazabicyclo[5.4.0]-7-undecene, manufactured by Tokyo Chemical Industry Co., Ltd.) was slowly added dropwise to the flask. After the addition was complete, the flask was capped and the contents were stirred at room temperature for 24 hours to obtain 40.0 g of reddish-brown liquid composite 1. (Synthesis Example 2: Composite 2) 30.0 g of reddish-brown liquid composite 2 was obtained in the same manner as Synthesis Example 1, except that 20 g of TC-750 (bis(ethylacetoacetate)diisopropoxytitanium, manufactured by Matsumoto Fine Chemical Co., Ltd.) was used. Synthesis Example 3: Composite 3 30.0 g of pale yellow liquid composite 3 was obtained in the same manner as in Synthesis Example 1, except that 20 g of TA-23 (butyl titanate dimer, manufactured by Matsumoto Fine Chemicam Co., Ltd.) was used.

[0138] (Method of Producing Curable Composition) (Examples 1 to 4 and Comparative Example 1) According to the composition (weight ratio) shown in Table 1, heavy calcium carbonate, colloidal calcium carbonate, plasticizer, pigment, thixotropy-imparting agent, antioxidant, UV absorber, and light stabilizer were added to organic polymer (A) and mixed using a spatula. The resulting mixture was passed through a triple paint roll (manufactured by Kodaira Seisakusho Co., Ltd.) three times to disperse it, and then dehydrated under reduced pressure using a planetary mixer to obtain a base resin. A silane compound and curing catalyst (B) shown in Table 1 were added to the base resin in this order and mixed to obtain a curable composition.

[0139] The components in Table 1 are as follows: Organic polymer (A) ((A-1) (organic polymer (A-1) obtained in Preparation Example 1)) Colloidal calcium carbonate (trade name: Hakuenka CCR, manufactured by Shiraishi Kogyo Co., Ltd.) Heavy calcium carbonate (trade name: Whiten SB, manufactured by Bihoku Funka Kogyo Co., Ltd.) Plasticizer (trade name: Hexamoll DINCH, manufactured by BASF) Pigment (trade name: Typec R820, manufactured by Ishihara Sangyo Kaisha, Ltd.) Thixotropic agent (trade name: Crayvallc SLT, manufactured by ARKEMA) Antioxidant (trade name: Irganox 1010, manufactured by BASF) Ultraviolet absorber (trade name: Tinuvin 326, manufactured by BASF) Light stabilizer (trade name: Tinuvin 770, manufactured by BASF) Amidine compound (b1) (DBU (1,8-diazabicyclo[5.4.0]undec-7-ene), manufactured by Tokyo Chemical Industry Co., Ltd.) Titanium compound (b2) (trade name: TC-750, manufactured by Matsumoto Fine Chemical Co., Ltd.) Silane condensate (C) (trade name: Dynasylan 6490, manufactured by Evonik) (trade name: Dynasylan 1146, manufactured by Evonik) Silane compounds other than silane condensate (C) (trade name: Dynasylan DAMO (γ-(2-aminoethyl)aminopropyltrimethoxysilane), manufactured by Evonik), (trade name: Dynasylan AMMO (γ-aminopropyltrimethoxysilane), manufactured by Evonik), (trade name: Dynasylan VTMO (vinyltrimethoxysilane), manufactured by Evonik)

[0140] (Skinning Time (Curability Evaluation)) The curable composition obtained above was filled into a moisture-proof container and stored for 7 days in an atmosphere of 23°C and 50% relative humidity. In an atmosphere of 23°C and 50% relative humidity, the curable composition was filled into a mold about 5 mm thick and the surface of the curable composition was smoothed to a flat surface. The time when the surface was smoothed to a flat surface was recorded as the curing initiation time. The curable composition in the mold was touched with a spatula, and the time when the mixture no longer adhered to the spatula was recorded as the skinning time, and the curing time (curability) was measured. The measurement results are shown in Table 1.

[0141]

[0142] From the measurement results in Table 1, a comparison between Examples 1 to 4 and Comparative Example 1 shows that the curable compositions containing the silane condensate (C) cure more quickly than the curable compositions not containing the silane condensate (C).

[0143] (Examples 5 to 22) According to the compositions (weight ratios) shown in Table 2, heavy calcium carbonate, colloidal calcium carbonate, plasticizer, pigment, thixotropy-imparting agent, antioxidant, UV absorber, and light stabilizer were added to organic polymer (A) and mixed using a spatula. The resulting mixture was passed through a triple paint roll (manufactured by Kodaira Seisakusho Co., Ltd.) three times to disperse the mixture, and then dehydrated under reduced pressure using a planetary mixer to obtain a base resin. The silane condensate (C) and curing catalyst (B) shown in Table 2 were added to the base resin in this order and mixed to obtain a curable composition.

[0144] The components in Table 2 are as follows. As the organic polymer (A), (A-1) (organic polymer (A-1) obtained in Preparation Example 1), (A-2) (organic polymer (A-2) obtained in Preparation Example 2), (A-3) (organic polymer (A-3) obtained in Preparation Example 3), (A-5) (organic polymer (A-5) obtained in Preparation Example 5), and (A-6) (organic polymer (A-6) obtained in Preparation Example 6) were used. As the colloidal calcium carbonate, Hakuenka CCR (manufactured by Shiraishi Kogyo Co., Ltd.) was used. As the heavy calcium carbonate, Whiten SB (manufactured by Bihoku Funka Kogyo Co., Ltd.) was used. As the plasticizer, Hexamoll DINCH (manufactured by BASF), DINP (diisononyl phthalate, manufactured by J-Plus Co., Ltd.), and Actcoal P-23 (manufactured by Mitsui Chemicals SKC Polyurethanes, Inc.) were used. As the pigment, Typec R820 (manufactured by Ishihara Sangyo Kaisha, Ltd.) was used. As the thixotropic agent, Crayvallc SLT (manufactured by ARKEMA) was used. As the antioxidant, Irganox 1010 (manufactured by BASF) was used. As the ultraviolet absorber, Tinuvin 326 (manufactured by BASF) was used. As the light stabilizer, Tinuvin 770 (manufactured by BASF) was used. As the amidine compound (b1), DBU (1,8-diazabicyclo[5.4.0]undec-7-ene), (manufactured by Tokyo Chemical Industry Co., Ltd.) was used. Examples of the titanium compound (b2) include TC-750 (bis(ethylacetoacetate)diisopropoxytitanium), manufactured by Matsumoto Fine Chemical Co., Ltd., Tyzor KE-6 (bis(ethylacetoacetate)diisobutoxytitanium), manufactured by Dorff Ketal, Tyzor 9000 (tetra tert-butoxytitanium), manufactured by Dorff Ketal, and Ti(O i Pr) 4 (tetraisopropoxytitanium), manufactured by Tokyo Chemical Industry Co., Ltd.) was used. Composite 1 is Composite 1 obtained in Synthesis Example 1. Composite 2 is Composite 2 obtained in Synthesis Example 2. Composite 3 is Composite 3 obtained in Synthesis Example 3. Dynasylan 6490 (manufactured by Evonik) and Dynasylan 1146 (manufactured by Evonik) were used as the silane condensate (C).

[0145] (Skinning Time (Curing Property Evaluation)) The curing time (curing property) was measured in the same manner as in Examples 1 to 4 and Comparative Example 1. The measurement results are shown in Table 2.

[0146]

[0147] The measurement results in Table 2 show that all of the curable compositions of Examples 5 to 22 containing the silane condensate (C) exhibit good rapid curing properties.

Claims

1. A curable composition comprising an organic polymer (A), a curing catalyst (B), and a silane condensate (C), wherein the organic polymer (A) is represented by the following formula (1): -SiR 1 X 2 (1) (In formula (1), R 1 is a hydrocarbon group having 1 to 20 carbon atoms, X is a hydroxyl group or a hydrolyzable group, and the two Xs may be the same or different; the curing catalyst (B) contains an amidine compound (b1) and a titanium compound (b2); the amidine compound (b1) is represented by the following formula (2): 2 N=CR 3 -NR 4 2 (2) (In formula (2), R 2 , R 3 , and R 4 is a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, and two R 4 may be the same or different, R 2 , R 3 , and two R 4 Any two of the groups may be bonded to form a ring. The titanium compound (b2) is a compound represented by the following formula (3): Ti(OR 5 ) d Y 4-d (3) (In formula (3), R 5 is a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, Y is a chelate coordination compound, and d is an integer of 0 to 4, or a condensate thereof, wherein the silane condensate (C) is a compound represented by the following formula (4): (In formula (4), R 6 is a methyl group or an ethyl group, R 6 may be the same or different, R 7 , R 8 is a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, R 7 , R 8 may be the same or different, and e and f are integers of 1 to 50.

2. The above R 6 The curable composition of claim 1 , wherein is a methyl group.

3. The curable composition according to claim 2, wherein the silane condensate (C) is a condensate of at least one kind of trimethoxysilane selected from vinyltrimethoxysilane, amino group-containing trimethoxysilane, and alkyltrimethoxysilane.

4. The curable composition according to any one of claims 1 to 3, wherein d in formula (3) is 0 or an integer of 1 to 3.

5. The curable composition according to any one of claims 1 to 3, wherein the main chain structure of the organic polymer (A) is polyoxyalkylene.

6. The curable composition according to any one of claims 1 to 3, wherein the amidine compound (b1) is DBU (1,8-diazabicyclo[5.4.0]-7-undecene).

7. The curable composition according to any one of claims 1 to 3, wherein the weight ratio (b2) / (b1) of the titanium compound (b2) to the amidine compound (b1) is 1.0 to 10.

Citation Information

Patent Citations

  • JP1971027250B1

  • Receiving device

    JP1984015336A

  • Production of polyalkylene oxide of narrow MW distribution

    JP1986197631A

  • Production of unsaturated group-terminated polyalkylene oxide

    JP1986215622A

  • Production of unsaturated group-terminated polyalkylene oxide

    JP1986215623A