Resin composition for optical imprint molds, and optical imprint mold

The resin composition for photoimprint molds, featuring a thermoplastic polymer with alicyclic structures and antioxidants, addresses the issues of light transmittance and brittleness in conventional thermoplastic resin molds, achieving high optical transparency and mechanical strength for optical imprinting.

WO2024203485A1PCT designated stage expired Publication Date: 2024-10-03ZEON CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010366
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-15
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional thermoplastic resin molds for optical imprinting lack sufficient light transmittance and mechanical strength, particularly at temperatures around the glass transition temperature plus 50°C, leading to brittleness and decreased transmittance, which hinders the formation of high-quality optical imprint molds with fine patterns.

Method used

A resin composition for photoimprint molds is developed, comprising a thermoplastic polymer with a nonpolar or halogen-containing alicyclic structure, combined with a high proportion of antioxidant (1.1-10% by weight), which is hydrogenated to achieve a glass transition temperature below 100°C, resulting in a mold with high light transmittance (>90% at 350-500 nm) and low brittleness.

Benefits of technology

The resin composition enables the creation of optical imprint molds with high light transmittance and low brittleness, maintaining these properties even after heating, thus effectively addressing the limitations of conventional thermoplastic resin molds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010366_03102024_PF_FP_ABST
    Figure JP2024010366_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide: a material for optical imprint molds that is capable of realizing high light transmittance and low brittleness; and an optical imprint mold that can exhibit these properties. Provided is a resin composition for optical imprint molds, which contains a polymer and an antioxidant, has an antioxidant content of 1.1-10 weight%, and is a thermoplastic resin composition. The polymer is preferably a nonpolar alicyclic structure-containing thermoplastic polymer, a halogen-containing alicyclic structure-containing thermoplastic polymer, or a mixture thereof, and more preferably is a hydrogenate of a ring-opening polymer of a cyclic olefin monomer. An optical imprint mold obtained by molding the resin composition is also provided.
Need to check novelty before this filing date? Find Prior Art

Description

Resin composition for photo-imprint mold and photo-imprint mold

[0001] The present invention relates to a resin composition for forming a mold for photo-imprinting, and to a photo-imprinting mold.

[0002] As a processing technology for forming fine uneven patterns, such as line-space patterns with widths of approximately 100 nm or less, on the surface of a flat material, a technology known as nanoimprinting is being considered as an alternative to lithography, which has been mainly used up until now. In nanoimprinting, a mold with a fine uneven shape is pressed against the surface of the material to be processed, thereby transferring the uneven shape.

[0003] Photoimprinting is known as a major nanoimprinting technique. In photoimprinting, a photocurable resin that can be cured by light such as ultraviolet light is brought into contact with the textured surface of a mold and then spread, and the photocurable resin is then irradiated with light to cure. In this case, to achieve good curing, the mold is required to be made of a material that has high transmittance for the light used to cure the photocurable resin. In particular, ultraviolet light of 350 nm to 500 nm, particularly around 350 nm, is often used to cure photocurable resins, so the mold is required to have good transmittance at such wavelengths.

[0004] Currently, standard molds for optical imprinting are manufactured through the following process: forming a layer of EB (electron beam) resist on single crystal glass, drawing with an electron beam, partially peeling off the resist, evaporating a metal such as chromium on the peeled-off area, peeling off the resist again, and then dry etching the glass in the peeled-off area.

[0005] In response to this, the use of photoimprinting molds made of thermoplastic resin instead of glass has been studied as a lower-cost mold (Patent Documents 1 to 3). Photoimprinting molds made of thermoplastic resin can be manufactured by thermal imprinting technology. Specifically, they are made by pressing a metal mold having a textured pattern against heated transparent thermoplastic resin to transfer the textured pattern.

[0006] JP 2011-111573 A, WO 2006 / 112062 A (corresponding publication: U.S. Patent Application No. 2009 / 057960), JP 2013-233807 A (corresponding publication: U.S. Patent Application No. 2006 / 279025),

[0007] Molds made of thermoplastic resins are required to have high optical transparency and mechanical strength. However, conventional molds made of thermoplastic resins do not fully meet these requirements, and therefore, there is a demand for optical imprint mold materials that can achieve even higher optical transparency and mechanical strength.

[0008] In particular, when a thermoplastic resin is a highly brittle material, chipping of the uneven shape easily occurs during molding and use of the mold, and therefore a material that is less brittle when molded into a mold is desired. However, conventional molds made of thermoplastic resins tend to become more brittle when exposed to temperatures such as the glass transition temperature (Tg) + 50°C during molding, and therefore a material that suppresses such an increase in brittleness is desired.

[0009] In particular, since molds are required to have good transmittance around 350 nm, materials that undergo little discoloration when formed into molds and when used as molds and that suppress a decrease in transmittance around this wavelength are required. However, conventional molds made of thermoplastic resins tend to have a decrease in transmittance around 350 nm when exposed to a temperature of, for example, the glass transition temperature (Tg) + 50°C during molding, so materials that suppress such a decrease in transmittance are required.

[0010] Therefore, an object of the present invention is to provide a material for a mold for optical imprinting that can achieve high optical transparency and low brittleness when formed into a mold, and an optical imprinting mold that can achieve such properties.

[0011] In order to solve the above problems, the present inventors have conducted research and found that the above problems can be solved by adding a high proportion of an antioxidant to a resin composition for photoimprint molding, which has not been done in the past, and have completed the present invention.

[0012] (1) A resin composition for photoimprint molding, which is a thermoplastic resin composition comprising a polymer and an antioxidant, the antioxidant content being 1.1 to 10% by weight. (2) The resin composition for photoimprint molding according to (1), wherein the polymer is a non-polar alicyclic structure-containing thermoplastic polymer, a halogen-containing alicyclic structure-containing thermoplastic polymer, or a mixture thereof. (3) The resin composition for photoimprint molding according to (2), wherein the polymer is a hydrogenated product of a ring-opening polymer of a cyclic olefin monomer. (4) The resin composition for photoimprint molding according to any one of (1) to (3), which has a glass transition temperature Tg of less than 100°C. (5) A photoimprint mold obtained by molding the resin composition for photoimprint molding according to any one of (1) to (4), wherein the light transmittance at a wavelength of 350 nm to 500 nm is 90% or more. (6) The photo-imprint mold according to (5), having a surface free energy of 40 mN / m or less.

[0013] According to the present invention, there are provided a material for a photo-imprinting mold that can achieve high optical transparency and low brittleness when formed into a mold, and a photo-imprinting mold that can achieve such properties.

[0014] Fig. 1 is a graph showing the relationship between the wavelength and transmittance of transmitted light for some of the Examples and Comparative Examples before and after heating for 30 minutes. Fig. 2 is a graph showing the relationship between the wavelength and transmittance of transmitted light for some of the Examples and Comparative Examples before and after heating for 30 minutes.

[0015] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and can be implemented with any modifications within the scope of the claims of the present invention and their equivalents.

[0016] (Outline of Thermoplastic Resin Composition) The resin composition of the present invention is a thermoplastic resin composition containing a polymer and a specific proportion of an antioxidant.

[0017] (Polymer) As the polymer that is a component of the resin composition, a polymer that is suitable as a material for a photoimprint mold, has high transparency, and when processed into the shape of a mold having fine irregularities by thermal imprinting, can be appropriately selected to give a molded product with low brittleness to such an extent that it can function as a mold. Examples of such polymers include non-polar alicyclic structure-containing thermoplastic polymers, halogen-containing alicyclic structure-containing thermoplastic polymers, and mixtures thereof.

[0018] The term "non-polar" refers to the absence of polar groups in the molecule. These polar groups are atomic groups containing atoms with unshared electron pairs, and can be divided into, for example, protic polar groups and other polar groups (aprotic polar groups).

[0019] The protic polar group is an atomic group in which a hydrogen atom is directly bonded to a heteroatom, specifically an atom in the second and third periods of Groups 15 and 16 of the periodic table.

[0020] Specific examples of protic polar groups include polar groups having an oxygen atom such as a carboxyl group (hydroxycarbonyl group), a sulfonic acid group, a phosphoric acid group, and a hydroxyl group; polar groups having a nitrogen atom such as a primary amino group, a secondary amino group, a primary amide group, and a secondary amide group (imide group); and polar groups having a sulfur atom such as a thiol group.

[0021] Specific examples of aprotic polar groups include those having an ester group (a general term for an alkoxycarbonyl group and an aryloxycarbonyl group), an N-substituted imide group, an epoxy group, a cyano group, a carbonyloxycarbonyl group (an acid anhydride residue of a dicarboxylic acid), an alkoxy group, a carbonyl group, a tertiary amino group, a sulfone group, an acryloyl group, etc. A halogen atom is usually incorporated into the aprotic polar group, but in the present invention, a thermoplastic polymer having a halogen-containing alicyclic structure can be used.

[0022] The non-polar alicyclic structure-containing thermoplastic polymer and halogen-containing alicyclic structure-containing thermoplastic polymer used in the present invention are polymers having structural units derived from cyclic olefin monomers such as norbornene structures, and may also have structural units derived from monomers other than cyclic olefin monomers.The alicyclic structure-containing thermoplastic polymer includes ring-opening polymers of cyclic olefin monomers (including homopolymers having a structure formed by ring-opening polymerization of a single type of monomer, copolymers having a structure formed by ring-opening copolymerization of multiple types of monomers, and mixtures thereof), addition copolymers of cyclic olefin monomers and vinyl alicyclic hydrocarbon monomers or vinyl aromatic hydrocarbon monomers, and hydrogenated products thereof.

[0023] The hydrogenated ring-opening polymer of a cyclic olefin monomer can easily give molded articles having good transmittance in the vicinity of 350 nm. The hydrogenated ring-opening polymer of a cyclic olefin monomer can also easily give molded articles having low surface free energy, which is particularly advantageous for forming molds with excellent releasability.

[0024] In the present invention, the term "alicyclic structure-containing thermoplastic polymer" refers to a concept that encompasses homopolymers and copolymers of vinyl alicyclic hydrocarbon monomers (alicyclic hydrocarbons having a vinyl group as a substituent), copolymers with other monomers, hydrogenated products thereof, polymers of vinyl aromatic hydrocarbon monomers (including homopolymers having a structure formed by polymerization of a single type of monomer, copolymers having a structure formed by copolymerization of multiple types of monomers, and mixtures thereof), and hydrogenated products of copolymers with other monomers. Furthermore, these polymers may be either ring-opening polymers or addition polymers. Among these, ring-opening polymers of cyclic olefin monomers and hydrogenated products thereof, addition copolymers of cyclic olefin monomers with vinyl alicyclic hydrocarbon monomers or vinyl aromatic hydrocarbon monomers and hydrogenated products thereof, and hydrogenated products of polymers of vinyl aromatic hydrocarbon monomers are preferred, with hydrogenated products of ring-opening polymers of cyclic olefin monomers being particularly preferred.

[0025] Examples of the cyclic olefin monomer for obtaining the non-polar alicyclic structure-containing thermoplastic polymer include the cyclic olefin monomers not having the polar group. Specific examples thereof include bicyclo[2.2.1]hept-2-ene (common name: norbornene), 5-ethyl-bicyclo[2.2.1]hept-2-ene, 5-butyl-bicyclo[2.2.1]hept-2-ene, 5-ethylidene-bicyclo[2.2.1]hept-2-ene, 5-methylidene-bicyclo[2.2.1]hept-2-ene, 5-vinyl-bicyclo[2.2.1]hept-2-ene, tricyclo[4.3.0.1]hept-2-ene, and the like. 2,5 ]deca-3,7-diene (common name: dicyclopentadiene), tetracyclo[8.4.0.1 11,14 .0 3,7 ] pentadeca-3,5,7,12,11-pentaene, tetracyclo[4.4.0.1 2,5 .1 7,10 ]dec-3-ene (common name: tetracyclododecene), 8-methyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ] dodec-3-ene, 8-ethyl-tetracyclo[4.4.0.1 2,5 .1 7,10] dodec-3-ene, 8-methylidene-tetracyclo[4.4.0.1 2,5 .1 7,10 ] dodec-3-ene, 8-ethylidene-tetracyclo[4.4.0.1 2,5 .1 7,10 ] dodec-3-ene, 8-vinyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ] dodec-3-ene, 8-propenyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ] dodec-3-ene, pentacyclo[6.5.1.1 3,6 .0 2,7 .0 9,13 ] pentadeca-3,10-diene, cyclopentene, cyclopentadiene, 1,4-methano-1,4,4a,5,10,10a-hexahydroanthracene, 8-phenyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ] dodec-3-ene, tetracyclo[9.2.1.0 2,10 .0 3,8 ]tetradeca-3,5,7,12-tetraene (also known as 1,4-methano-1,4,4a,9a-tetrahydro-9H-fluorene), pentacyclo[7.4.0.1 3,6 .1 10,13 .0 2,7 ] pentadeca-4,11-diene, pentacyclo[9.2.1.1 4,7 .0 2,10 .0 3,8 ]pentadeca-5,12-diene, and the like.

[0026] Examples of the cyclic olefin monomer for obtaining the halogen-containing alicyclic structure-containing thermoplastic polymer include cyclic olefin monomers containing halogen atoms. 2,5 .1 7,10 ] dodec-3-ene, 8-methyl-8-chlorotetracyclo[4.4.0.1 2,5 .1 7,10 ]dodec-3-ene, and the like.

[0027] In the present invention, the cyclic olefin monomer having no polar group and the cyclic olefin monomer having a halogen atom may be used alone or in combination of two or more thereof, and among these, norbornene is preferred.

[0028] Examples of the vinyl alicyclic hydrocarbon monomer include vinylcycloalkanes such as vinylcyclopropane, vinylcyclobutane, vinylcyclopentane, vinylcyclohexane, and vinylcycloheptane; and alkyl group-substituted vinylcycloalkanes such as 3-methyl-1-vinylcyclohexane, 4-methyl-1-vinylcyclohexane, 1-phenyl-2-vinylcyclopropane, and 1,1-diphenyl-2-vinylcyclopropane.

[0029] Examples of the vinyl aromatic hydrocarbon monomer include vinyl aromatics such as styrene, 1-vinylnaphthalene, 2-vinylnaphthalene, and 3-vinylnaphthalene; alkyl group-substituted vinyl aromatics such as 3-methylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, and 4-(phenylbutyl)styrene; and polyfunctional vinyl aromatics such as m-divinylbenzene, p-divinylbenzene, and bis(4-vinylphenyl)methane.

[0030] Other typical examples of monomers copolymerizable with cyclic olefins include chain olefins. Examples of the chain olefin include ethylene, α-olefins having 2 to 20 carbon atoms such as propylene, 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene, and non-conjugated dienes such as 1,4-hexadiene, 4-methyl-1,4-hexadiene, 5-methyl-1,4-hexadiene, and 1,7-octadiene. These monomers can be used alone or in combination of two or more.

[0031] The polymerization of each of the above monomers can be carried out according to conventional methods. For example, ring-opening polymerization and addition polymerization are employed. Metal complexes of molybdenum, ruthenium, osmium, and the like are preferably used as polymerization catalysts. These polymerization catalysts can be used alone or in combination of two or more. The amount of polymerization catalyst, in terms of the molar ratio of metal compound to cyclic olefin in the polymerization catalyst, is usually in the range of 1:100 to 1:2,000,000, preferably 1:500 to 1:1,000,000, and more preferably 1:1,000 to 1:500,000.

[0032] The cyclic olefin polymer obtained by the above polymerization may be hydrogenated, if necessary. Hydrogenation is usually carried out using a hydrogenation catalyst. As the hydrogenation catalyst, for example, a catalyst generally used in the hydrogenation of olefin compounds can be used. Specifically, Ziegler-type homogeneous catalysts, noble metal complex catalysts, and supported noble metal catalysts can be used. Among these hydrogenation catalysts, noble metal complex catalysts such as rhodium and ruthenium are preferred, and ruthenium catalysts coordinated with highly electron-donating nitrogen-containing heterocyclic carbene compounds or phosphines are particularly preferred.

[0033] The weight average molecular weight (Mw) of the alicyclic structure-containing thermoplastic polymer is usually in the range of 1,000 to 1,000,000, preferably 1,500 to 100,000, and more preferably 2,000 to 10,000. Furthermore, the molecular weight distribution of this thermoplastic polymer, expressed as a weight average molecular weight / number average molecular weight (Mw / Mn) ratio, is usually 4 or less, preferably 3 or less, and more preferably 2.5 or less. The weight average molecular weight (Mw) and number average molecular weight (Mw) are values ​​measured by gel permeation chromatography (GPC) using cyclohexane (or toluene) as a solvent, converted into polyisoprene (however, when toluene is used as the solvent, converted into polystyrene).

[0034] The glass transition temperature (Tg) of the polymer used in the present invention can be adjusted to a temperature suitable for use as a mold by appropriately adjusting the type and composition of the monomer. The glass transition temperature is preferably 60°C or higher, more preferably 65°C or higher, and is preferably 160°C or lower, more preferably lower than 100°C. In the present application, the glass transition temperature can be specifically measured by the measurement method shown in the examples of the present application.

[0035] The proportion of the polymer in the resin composition of the present invention is preferably sufficiently high from the viewpoint of exhibiting good properties as a mold. Specifically, the proportion of the polymer in 100% by weight of the resin composition is preferably 80% by weight or more, more preferably 90% by weight or more, while the upper limit is 98.9% by weight or less. In particular, it is preferable that the content ratios of the non-polar alicyclic structure-containing thermoplastic polymer and the halogen-containing alicyclic structure-containing thermoplastic polymer are within this range, and furthermore, it is preferable that the content ratio of the hydrogenated product of the ring-opening polymer of the cyclic olefin monomer is within this range.

[0036] (Antioxidant) The antioxidant is added to prevent the resin composition of the present invention from being degraded when the resin composition is molded into a mold and when the mold is used. As the antioxidant, a hindered phenol-based antioxidant can be preferably used.

[0037] Hindered phenol antioxidants are compounds having a molecular structure in which one or two of the benzene ring substitution positions adjacent to the OH group of phenol have substituents capable of causing steric hindrance. Examples of such substituents include branched alkyl groups having 3 to 10 carbon atoms, preferably t-butyl groups. More specific examples of compounds that are hindered phenol antioxidants include compounds having a molecular structure containing one or more 4-hydroxy-3,5-dialkylphenyl groups, and even more specific examples include compounds having a molecular structure containing one or more 3,5-di-t-butyl-4-hydroxyphenyl groups. An even more specific example of such an antioxidant is pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (trade name "Irganox 1010", manufactured by BASF).

[0038] The proportion of the antioxidant in 100% by weight of the resin composition of the present invention is 1.1% by weight or more, preferably 2.9% by weight or more, and 10% by weight or less, preferably 6% by weight or less. Conventionally, a large amount of antioxidant, such as 1.1% by weight or more, has not been added to resin compositions for photoimprint molding. However, the present inventors have found that adding such a high concentration of antioxidant can suppress an increase in brittleness and a decrease in transmittance at around 350 nm when the resin composition is placed at a temperature of the glass transition temperature Tg + 50°C, which is the temperature at which the resin composition is formed into a mold, and can also suppress a decrease in transmittance at around 350 nm.

[0039] (Other Components) The resin composition of the present invention may contain any additive components in addition to the polymer and antioxidant. Examples of these various additive components include a mold release agent, a heat stabilizer, a light stabilizer, a lubricant, an antistatic agent, a dye, a colorant, an antiblocking agent, a natural oil, a synthetic oil, a wax, a flame retardant, a flame retardant aid, a compatibilizer, a crosslinking agent, a crosslinking aid, and a plasticizer.

[0040] (Method for Producing Resin Composition) The method for producing the resin composition is not particularly limited, and any known method can be adopted. Specifically, the resin composition can be produced by melting a material containing the above-described polymer by heating or the like, and mixing it with an antioxidant and, if added, any optional additive components.

[0041] (Physical Properties of Resin Composition) Since the resin composition of the present invention is mainly composed of a polymer, the glass transition temperature of the resin composition can be equivalent to that of the polymer described above. Specifically, the glass transition temperature (Tg) of the resin composition is preferably 60°C or higher, more preferably 65°C or higher, and is preferably 160°C or lower, more preferably lower than 100°C. When a resin composition having a glass transition temperature in this range is molded at a temperature suitable for molding, such as Tg + 50°C, it is particularly advantageous to suppress an increase in brittleness and a decrease in transmittance.

[0042] From the viewpoint of maintaining performance when molded into a photo-imprint mold, the resin composition of the present invention is preferably a transparent material with high light transmittance. Specifically, when molded into a plate-like article having a thickness of 100 μm, the light transmittance is preferably 90% or more over the entire wavelength range of 350 to 500 nm. A resin composition having such high light transmittance can be obtained by appropriately selecting a polymer from a non-polar alicyclic structure-containing thermoplastic polymer, a halogen-containing alicyclic structure-containing thermoplastic polymer, or a mixture thereof. The upper limit of the light transmittance is ideally 100%, but it can also be less than 100%.

[0043] (Photo-imprint mold) The resin composition of the present invention is a resin composition for photo-imprint molds. The photo-imprint mold of the present invention is obtained by molding the resin composition for photo-imprint molds of the present invention.

[0044] The molding method is not particularly limited, and molding can be performed using known thermal imprinting techniques. Specifically, molding can be performed by pressing a master mold, such as a mold having a concave-convex shape, against a heated thermoplastic resin in a plate shape to transfer the concave-convex shape of the master mold. The preferred range of the heating temperature during molding can be defined as a value relative to the glass transition temperature Tg of the resin composition. Although it also depends on the thickness and area of ​​the mold to be used, specifically, the preferred heating temperature can be preferably within the range of Tg + 40°C to Tg + 60°C, more preferably within the range of Tg + 45°C to Tg + 55°C.

[0045] The shape of the photo-imprint mold is usually a substantially flat plate-like molded product, with the concave-convex shape transferred to its main surface. The thickness of the plate-like molded product can be adjusted appropriately depending on the desired mode of use, but is preferably 50 μm to 200 μm, more preferably 80 μm to 120 μm.

[0046] The photoimprint mold of the present invention preferably has a light transmittance of 90% or more in the wavelength range of 350 to 500 nm. In other words, the photoimprint mold of the present invention may have a light transmittance of 90% or more in the entire wavelength range of 350 to 500 nm. In photoimprinting, light is generally irradiated from the surface of the mold opposite the surface having the textured structure. Therefore, a high transmittance of light in this range, which is a wavelength suitable for light irradiation, is particularly advantageous for the mold. The light transmittance can be measured as the transmittance of light transmitted perpendicularly from one main surface of the mold to the other main surface. Specifically, the light transmittance can be measured by the measurement method shown in the Examples of the present application. In particular, when a plate-shaped molded product serving as the master plate of the mold is obtained using the resin composition of the present invention and a textured structure is transferred to the mold by thermal imprinting, a mold having a high light transmittance of 90% or more can be obtained even when the thermal imprinting operation is performed in an atmosphere prone to yellowing. The upper limit of light transmittance is ideally 100%, but may be less than 100%.

[0047] When transferring the relief structure to a plate-shaped molded article, the molded article is heated at the heating temperature described above. Therefore, it is preferable that the photo-imprint mold of the present invention maintains the above-described light transmittance after being heated and molded at such a heating temperature. Specifically, it is preferable that the above-described light transmittance is maintained even when the plate-shaped molded article is heated at a temperature of Tg + 50°C for a period of time longer than a certain period of time. The heating time is preferably 10 minutes or more, more preferably 30 minutes or more. Since a longer heating time during which the light transmittance is maintained is preferable, the upper limit is not particularly limited. For example, if the light transmittance is maintained even after measurement for one hour, it can be evaluated as having sufficient durability without requiring a longer measurement period.

[0048] The photo-imprinting mold of the present invention preferably has a low surface free energy. A mold with a low surface free energy has excellent releasability and is particularly advantageous in carrying out photo-imprinting. The surface free energy of the photo-imprinting mold is preferably 40 mN / m or less, more preferably 38 mN / m or less. The lower limit of the surface free energy is not particularly limited, but can be 30 mN / m or more. Specifically, the measurement and calculation of the surface free energy can be carried out by the measurement methods and calculation methods shown in the examples of the present application.

[0049] The photo-imprint mold of the present invention can be used when performing photo-imprinting in the manufacture of products that require fine processing, such as various optical devices and integrated circuit components.

[0050] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the following examples and can be modified as desired without departing from the scope of the claims and their equivalents. In the following description, "%" and "parts" representing amounts are by weight unless otherwise specified. Furthermore, the operations described below were performed in air at room temperature and normal pressure unless otherwise specified. In the following evaluations, surface free energy, light transmittance, and other evaluations were performed on resin compositions molded into plates. The plate-shaped molded product differs from the mold actually used in that it does not have an uneven shape. However, since it is heated under heating conditions equivalent to or more severe than the heating conditions for molding the mold, it can be used as an indicator of the physical properties of the mold.

[0051] [Evaluation Method] (Glass Transition Temperature Tg of Resin Composition) The glass transition temperature (Tg) of the sample was measured using a differential scanning calorimeter (manufactured by SII Nanotechnology Inc., product name: DSC6220) at a temperature rise rate of 10°C / min in accordance with JIS K 6911.

[0052] (Surface Free Energy of Resin Composition Molded Article) The surface free energy of the resin composition molded article was determined by measuring the contact angle of water and diiodomethane on the flat surface of the molded article. From the measured contact angle values ​​and known physical property values ​​of water and diiodomethane, the contact angle of water of the molded article and the contact angle of diiodomethane (CH 2 I 2 The contact angle of the adhesive was measured using a Kyowa Interface Science DMo-502 and used as an index of surface free energy. (Reference: Journal of the Japan Welding Society, Vol. 81 (2012), No. 6, "Fundamentals of Adhesion")

[0053] (Color Change of Resin Composition Molded Article) The plate-shaped molded article to be evaluated was visually observed with the naked eye, and the degree of yellowing was evaluated into four levels: "yellowing," "slight yellowing," "slight yellowing," and "no change."

[0054] (Light transmittance of resin composition molded article) The light transmittance of the plate-shaped molded article to be evaluated was measured using a V-7200 manufactured by JASCO Corporation. The relationship between the wavelength of transmitted light and the transmittance was recorded.

[0055] (Brittleness of resin composition molded article) A plate-shaped molded article was cut out to prepare a rectangular test piece measuring 3 cm x 6 cm. A metal rod with a radius of 1 mm was held with its axis horizontal, and the test piece was placed on top of it. The test piece was placed so that the center of the longitudinal direction of the test piece was in contact with the metal rod and the width direction of the test piece was parallel to the axis of the metal rod. Next, an equal downward force was applied to both ends of the test piece to bend the test piece. The state of the test piece when it was bent 90° was observed and evaluated according to the following evaluation criteria. A: The test piece did not crack, and no white streaks occurred at the bent portion. B: The test piece did not crack, but white streaks occurred at the bent portion. C: The test piece cracked.

[0056] (Examples 1-1 to 1-3, Comparative Examples 1-1 to 1-4, Examples 2-1 to 2-3, and Comparative Examples 2-1 to 2-4) A resin containing a hydrogenated ring-opening polymer of a cyclic olefin monomer was melted at approximately 270°C and immediately mixed with an antioxidant (product name "Irganox 1010" manufactured by BASF) after melting to obtain a resin composition for photoimprint molding. In Examples 1-1 to 1-3 and Comparative Examples 1-1 to 1-4, the product name "Zeonex 5000" (manufactured by Zeon Corporation) was used as the hydrogenated cyclic olefin polymer resin, and in Examples 2-1 to 2-3 and Comparative Examples 2-1 to 2-4, the product name "ZF16" (manufactured by Zeon Corporation) was used as the cyclic olefin polymer resin. The proportion of antioxidant in the resin composition was as shown in Table 1.

[0057] After mixing, the resin composition was cooled to room temperature and cured to form a plate-shaped molded article having a thickness of 100 μm. The glass transition temperature Tg of the obtained resin composition was 80°C in all of Examples 1-1 to 1-3 and Comparative Examples 1-1 to 1-4, and 160°C in all of Examples 2-1 to 2-3 and Comparative Examples 2-1 to 2-4. When the molded articles of the obtained resin composition were visually observed, they were all transparent objects. When the transmittance at 350 nm was measured using the obtained molded articles of the resin composition as samples, all were 90%.

[0058] Surface free energy was measured using a molded article of the obtained resin composition as a sample. Furthermore, a plate-shaped molded article of the obtained resin composition was heat-treated at a temperature of Tg + 50°C for 10 minutes or 30 minutes. The degree of yellowing, 350 nm absorbance, and brittleness of the treated plate-shaped molded article were evaluated. The evaluation results are shown in Table 1. Furthermore, for some of the Examples and Comparative Examples, the relationship between the wavelength of transmitted light and the transmittance before and after 30 minutes of heating is shown in Figures 1 and 2. In addition to those shown in Figures 1 and 2, in all of Examples 1-1 to 1-3 and Examples 2-1 to 2-3, the transmittance was 90% or higher at all wavelengths from 350 nm to 500 nm before heating and after 10 minutes of heating. Furthermore, in Examples 1-2 to 1-3 and Examples 2-2 to 2-3, the transmittance was 90% or higher at all wavelengths from 350 nm to 500 nm even after 30 minutes of heating.

[0059]

[0060] From the above results, it can be seen that in the examples that satisfy the requirements of the present invention, low surface free energy that is useful as a mold can be achieved, and that high light transmittance and low brittleness can be achieved even in the plate-shaped molded product after heating that corresponds to the state of the photo-imprint mold.

Claims

1. A resin composition for photoimprint molding, which is a thermoplastic resin composition comprising a polymer and an antioxidant, the antioxidant content being 1.1 to 10% by weight.

2. The resin composition for photoimprint molding according to claim 1, wherein the polymer is a non-polar alicyclic structure-containing thermoplastic polymer, a halogen-containing alicyclic structure-containing thermoplastic polymer, or a mixture thereof.

3. The resin composition for photoimprint molding according to claim 2, wherein the polymer is a hydrogenated product of a ring-opening polymer of a cyclic olefin monomer.

4. The resin composition for photoimprint molding according to claim 1, which has a glass transition temperature Tg of less than 100°C.

5. A photoimprint mold obtained by molding the resin composition for photoimprint molds according to any one of claims 1 to 4, wherein the photoimprint mold has a light transmittance of 90% or more at wavelengths of 350 nm to 500 nm.

6. The photoimprint mold according to claim 5, having a surface free energy of 40 mN / m or less.

Citation Information

Patent Citations

  • Mold or stamper made of resin

    JP2005288803A

  • Manufacturing method of optical element and processing method of mold for optical element

    JP2006076235A

  • Thermoplastic resin particle composition, thermoplastic resin molding using the composition, and method for producing the molding

    JP2010173144A

  • Imprinting mold

    JP2012143915A

  • Form, microprocessed article, and their manufacturing methods

    WO2008149544A1