Pressure-sensitive adhesive sheet

The adhesive sheet, with its specific polymer and tackifier composition, addresses the issue of low-temperature bending resistance and adhesiveness, ensuring durability and reliability in flexible display applications by maintaining strong adhesion across a wide temperature range.

WO2024203546A1PCT designated stage expired Publication Date: 2024-10-03NITTO DENKO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010577
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional adhesive sheets exhibit poor bending resistance at low temperatures, which compromises their adhesiveness and durability in flexible display applications, where repeated bending occurs across various environmental conditions.

Method used

A pressure-sensitive adhesive sheet with a pressure-sensitive adhesive layer containing an acrylic polymer and a tackifier, featuring an elastic modulus of 5.0 MPa or less at -30°C and a gel fraction of 50% or higher, utilizing (meth)acrylic acid alkyl esters with linear or branched alkyl groups of 10 or more carbon atoms, and optionally including (meth)acrylic acid alkyl esters with 1 to 8 carbon atoms, to maintain adhesiveness across a wide temperature range.

Benefits of technology

The adhesive sheet demonstrates excellent bending resistance in low-temperature environments and retains strong adhesiveness from room temperature to high temperatures, preventing peeling and marks even under repeated bending, thus ensuring reliable performance in flexible display applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010577_03102024_PF_FP_ABST
    Figure JP2024010577_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a pressure-sensitive adhesive sheet which has excellent flex resistance in a low-temperature environment and, despite this, has excellent tackiness in a wide temperature range from ordinary temperature to high temperatures. The pressure-sensitive adhesive sheet 1 includes a pressure-sensitive adhesive layer 2. The pressure-sensitive adhesive layer 2 comprises: an acrylic polymer including, as a constituent unit, an alkyl (meth)acrylate having a C10 or higher, linear or branched, alkyl group; and a tackifier. The pressure-sensitive adhesive layer 2 has a -30°C elastic modulus of 5.0 MPa or less and a gel fraction of 50% or higher.
Need to check novelty before this filing date? Find Prior Art

Description

adhesive sheet

[0001] The present invention relates to a pressure-sensitive adhesive sheet.

[0002] Pressure-sensitive adhesive sheets used in image display devices and portable electronic devices such as mobile phones, smartphones, digital cameras, liquid crystal displays (LCDs), and organic EL displays are required to have a variety of performance characteristics, including high adhesive strength.

[0003] In recent years, organic EL panels using foldable substrates (flexible substrates) such as resin films have been put to practical use, and foldable flexible displays have been proposed. In flexible displays, not only are display panels such as organic EL panels foldable, but also their constituent members, which are bonded together via adhesive sheets. In foldable flexible displays (foldable displays), bending is performed repeatedly at the same location. At the bending point, compressive stress is applied to the inside and tensile stress to the outside, causing distortion at the bending point and its surroundings, which raises concerns about creases or marks at the bending point or peeling of the adhesive layer.

[0004] For example, Patent Documents 1 to 7 disclose pressure-sensitive adhesive sheets that are intended to have bending resistance.

[0005] JP 2018-111754 A JP 2019-108498 A JP 2020-111734 A JP 2020-139034 A JP 2020-164575 A JP 2018-27996 A JP 2019-218513 A

[0006] Considering the possibility that flexible displays will be used worldwide, it is not enough for them to have excellent flex resistance only at room temperature in Japan, and they are required to have excellent flex resistance in a variety of environments. However, conventional pressure-sensitive adhesive sheets may have poor flex resistance at low temperatures even if they have flex resistance at room temperature.

[0007] In order to improve the bending resistance at low temperatures, it is conceivable to use a polymer with a low glass transition temperature as the base polymer in the adhesive layer constituting the adhesive sheet. However, in this case, the elastic modulus at high temperatures decreases as well as the elastic modulus at low temperatures, resulting in a decrease in cohesive force at high temperatures, which reduces the adhesiveness and makes the sheet more susceptible to peeling. For this reason, it has been difficult to produce an adhesive sheet that has excellent bending resistance at low temperatures and excellent adhesiveness at high temperatures.

[0008] The present invention was conceived under these circumstances, and its purpose is to provide an adhesive sheet that has excellent flex resistance in low-temperature environments and excellent adhesiveness over a wide temperature range from room temperature to high-temperature environments.

[0009] As a result of extensive research to achieve the above object, the present inventors have found that a specific pressure-sensitive adhesive sheet has excellent flex resistance in low-temperature environments, while also having excellent adhesiveness over a wide temperature range from room temperature to high-temperature environments. The present invention was completed based on these findings.

[0010] That is, the present invention provides a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer, wherein the pressure-sensitive adhesive layer comprises an acrylic polymer containing, as a constituent unit, a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms, and a tackifier, and the pressure-sensitive adhesive layer has an elastic modulus of 5.0 MPa or less at −30° C. and a gel fraction of 50% or more.

[0011] The acrylic polymer preferably contains, as a constituent unit, an alkyl (meth)acrylate ester having a linear or branched alkyl group having 1 to 8 carbon atoms.

[0012] The tackifier preferably comprises an oligomer or a tackifying resin.

[0013] The pressure-sensitive adhesive sheet may be a double-sided pressure-sensitive adhesive sheet for fixing components together in an electric or electronic device.

[0014] The present invention also provides an electric / electronic device comprising the above-mentioned pressure-sensitive adhesive sheet, wherein the pressure-sensitive adhesive sheet fixes components together using both adhesive surfaces thereof.

[0015] The pressure-sensitive adhesive sheet of the present invention has excellent flex resistance in low-temperature environments and excellent adhesiveness over a wide temperature range from room temperature to high temperatures. Therefore, even when used in a location where repeated bending occurs in a low-temperature environment, the pressure-sensitive adhesive sheet is unlikely to crease or mark at the bending location or peel off.

[0016] 1 is a cross-sectional view of a pressure-sensitive adhesive sheet according to one embodiment of the present invention.

[0017] [Adhesive Sheet] A pressure-sensitive adhesive sheet according to one embodiment of the present invention includes at least a pressure-sensitive adhesive layer that contains an acrylic polymer and a tackifier, and has an elastic modulus of 5.0 MPa or less and a gel fraction of 50% or more at −30° C. In this specification, the pressure-sensitive adhesive layer may be referred to as the “pressure-sensitive adhesive layer of the present invention.”

[0018] The pressure-sensitive adhesive sheet of the present invention may be a so-called "substrate-less" pressure-sensitive adhesive sheet that does not have a substrate (substrate layer), or may be a pressure-sensitive adhesive sheet that has a substrate. In this specification, a "substrate-less" pressure-sensitive adhesive sheet may be referred to as a "substrate-less pressure-sensitive adhesive sheet," and a pressure-sensitive adhesive sheet that has a substrate may be referred to as a "substrate-attached pressure-sensitive adhesive sheet." Examples of the substrate-less pressure-sensitive adhesive sheet include a double-sided pressure-sensitive adhesive sheet consisting only of the pressure-sensitive adhesive layer of the present invention, and a double-sided pressure-sensitive adhesive sheet consisting of the pressure-sensitive adhesive layer of the present invention and another pressure-sensitive adhesive layer (a pressure-sensitive adhesive layer other than the pressure-sensitive adhesive layer of the present invention). Examples of the substrate-attached pressure-sensitive adhesive sheet include a single-sided pressure-sensitive adhesive sheet having the pressure-sensitive adhesive layer of the present invention on one side of the substrate, a double-sided pressure-sensitive adhesive sheet having the pressure-sensitive adhesive layer of the present invention on both sides of the substrate, and a double-sided pressure-sensitive adhesive sheet having the pressure-sensitive adhesive layer of the present invention on one side of the substrate and another pressure-sensitive adhesive layer on the other side. The "substrate (substrate layer)" refers to a support, and is the part that is attached to the adherend together with the pressure-sensitive adhesive layer when the pressure-sensitive adhesive sheet of the present invention is used (attached) to the adherend. The release liner that is peeled off when the pressure-sensitive adhesive sheet is used (applied) is not included in the above substrate.

[0019] Fig. 1 is a cross-sectional schematic diagram showing one embodiment of a pressure-sensitive adhesive sheet of the present invention. The pressure-sensitive adhesive sheet 1 shown in Fig. 1 is a substrate-less double-sided pressure-sensitive adhesive sheet consisting of a single pressure-sensitive adhesive layer 2 that is the pressure-sensitive adhesive layer of the present invention, and release liners 3 and 4 are provided on both pressure-sensitive adhesive surfaces, respectively.

[0020] (Pressure-sensitive adhesive layer of the present invention) The pressure-sensitive adhesive sheet of the present invention may have only one pressure-sensitive adhesive layer, or may have two or more pressure-sensitive adhesive layers. When two or more layers are included, at least one layer needs to be the pressure-sensitive adhesive layer of the present invention, and the other pressure-sensitive adhesive layers may be the pressure-sensitive adhesive layer of the present invention or other pressure-sensitive adhesive layers. When two or more pressure-sensitive adhesive layers of the present invention are included, the multiple pressure-sensitive adhesive layers of the present invention may be the same pressure-sensitive adhesive layer, or may be pressure-sensitive adhesive layers with different compositions, thicknesses, physical properties, etc. Furthermore, in the case of a pressure-sensitive adhesive sheet with a substrate, the pressure-sensitive adhesive layer provided on one side of the substrate may be a single layer, or may be a multilayer composed of layers that are the same or have different compositions, thicknesses, physical properties, etc.

[0021] The pressure-sensitive adhesive layer of the present invention has a modulus of elasticity at -30°C of 5.0 MPa or less, preferably 4.0 MPa or less, more preferably 3.0 MPa or less, even more preferably 2.0 MPa or less, and particularly preferably 1.0 MPa or less. By having the modulus of elasticity of 5.0 MPa or less, even when repeatedly bent at low temperatures, the pressure-sensitive adhesive layer is less likely to develop creases or marks at bent locations or peel off, resulting in excellent flex resistance. The modulus of elasticity is, for example, 0.1 MPa or more, preferably 0.2 MPa or more.

[0022] In this specification, the "elastic modulus" refers to the dynamic shear storage modulus (G'), which can be measured, for example, using a viscoelasticity tester in a shear mode at a temperature range of -50 to 150°C and a heating rate of 5°C / min while applying a shear strain at a frequency of 1 Hz, and the peak G' at any temperature can be obtained as the elastic modulus.

[0023] The gel fraction (mass proportion of solvent-insoluble components) of the pressure-sensitive adhesive layer of the present invention is 50% or more, preferably 60% or more, and more preferably 70% or more. A gel fraction of 50% or more improves the cohesive strength of the pressure-sensitive adhesive layer, resulting in excellent adhesion to the adherend in a high-temperature environment. The gel fraction is, for example, 95% or less, preferably 90% or less. A gel fraction of 95% provides adequate flexibility and further improves adhesion. The gel fraction can be controlled, for example, by the monomer composition of the acrylic polymer, the weight-average molecular weight, the amount of crosslinking agent used (added), etc.

[0024] Specifically, the gel fraction is a value calculated, for example, by the "Method for Measuring Gel Fraction" below. (Method for Measuring Gel Fraction) Approximately 0.2 g of the pressure-sensitive adhesive layer is collected from the pressure-sensitive adhesive sheet, wrapped in a porous tetrafluoroethylene sheet (trade name "NTF1122", manufactured by Nitto Denko Corporation) having an average pore size of 0.2 μm, and then tied with kite string. The mass at this time is measured, and this mass is defined as the pre-immersion mass. The pre-immersion mass is the total mass of the mass (B) of the pressure-sensitive adhesive layer (the pressure-sensitive adhesive layer collected above), the mass of the tetrafluoroethylene sheet, and the mass of the kite string. The total mass of the tetrafluoroethylene sheet and the kite string is also measured, and this mass is defined as the wrapping mass (A). Next, the pressure-sensitive adhesive layer wrapped in the tetrafluoroethylene sheet and tied with the kite string (referred to as the "sample") is placed in a 50 ml container filled with ethyl acetate and allowed to stand at 23° C. for 7 days. The sample (after ethyl acetate treatment) was then removed from the container, transferred to an aluminum cup, and dried in a dryer at 130°C for 2 hours to remove the ethyl acetate. The mass was then measured and used as the post-immersion mass (C). The gel fraction was then calculated using the following formula: Gel fraction [mass %] = 100 × (C - A) / B

[0025] The pressure-sensitive adhesive layer of the present invention preferably has a 180° peel adhesion strength against a SUS flat surface at room temperature of 5.0 N / 20 mm or more, more preferably 5.5 N / 20 mm or more, and more preferably 6.0 N / 20 mm or more. When the peel adhesion strength is 5.0 N / 20 mm or more, the pressure-sensitive adhesive sheet is less likely to peel even when repeatedly bent at around room temperature, and has excellent flex resistance. The higher the peel adhesion strength, the less likely peeling occurs, but it is, for example, 20.0 N / 20 mm or less. The room temperature refers to an environment of, for example, a temperature of 23°C and a relative humidity of 50% RH.

[0026] The pressure-sensitive adhesive layer of the present invention is a pressure-sensitive adhesive layer containing an acrylic polymer. The pressure-sensitive adhesive layer of the present invention is preferably an acrylic pressure-sensitive adhesive layer containing an acrylic polymer as a base polymer that exhibits adhesiveness. In this specification, the base polymer refers to the main component of the polymer components in the pressure-sensitive adhesive that constitutes the pressure-sensitive adhesive layer, for example, a polymer component that is contained in an amount of more than 50% by mass. The content of the base polymer in the pressure-sensitive adhesive layer is preferably 60% by mass or more, more preferably 70% by mass or more, relative to 100% by mass of the total amount of the pressure-sensitive adhesive layer.

[0027] The pressure-sensitive adhesive layer of the present invention contains at least an acrylic polymer containing, as a constituent unit, a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms, and a tackifier. The acrylic polymer may be referred to as the "acrylic polymer of the present invention." The pressure-sensitive adhesive layer of the present invention may contain only one type of acrylic polymer of the present invention, or may contain two or more types.

[0028] The acrylic polymer of the present invention is a polymer containing an acrylic monomer (a monomer having a (meth)acryloyl group in the molecule) as a monomer component constituting the polymer. That is, the acrylic polymer contains structural units derived from the acrylic monomer. Only one type of acrylic polymer may be used, or two or more types may be used. Furthermore, the acrylic polymer may contain only one type of acrylic monomer as a monomer component, or two or more types. In this specification, "(meth)acrylic" refers to "acrylic" and / or "methacrylic" (either one or both of "acrylic" and "methacrylic"), and the same applies to other terms.

[0029] The acrylic polymer of the present invention contains the above-mentioned (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms as a constituent unit. As a result, the pressure-sensitive adhesive sheet of the present invention has excellent flex resistance in low-temperature environments without reducing adhesiveness at room temperature and high-temperature environments. The above-mentioned (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms may be used alone or in combination of two or more.

[0030] Examples of the (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms include decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (lauryl (meth)acrylate), tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate.

[0031] In the alkyl (meth)acrylate having a linear or branched alkyl group having 10 or more carbon atoms, the alkyl group preferably has 10 to 18 carbon atoms, and more preferably 12 to 16 carbon atoms.

[0032] The proportion of the (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms in all monomer components constituting the acrylic polymer of the present invention is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, relative to the total amount (100% by mass) of all monomer components. Furthermore, from the viewpoint of copolymerizing other monomer components and obtaining the effects of the other monomer components, the proportion may be 70% by mass or less, 60% by mass or less, 50% by mass or less, 20% by mass or less, 16% by mass or less, or 10% by mass or less.

[0033] The acrylic polymer of the present invention preferably further contains, as a structural unit, a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 1 to 8 carbon atoms. This provides the pressure-sensitive adhesive sheet of the present invention with superior adhesiveness at room temperature and in high temperature environments. The (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 1 to 8 carbon atoms may be used alone or in combination of two or more types.

[0034] Examples of the (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 1 to 8 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isooctyl (meth)acrylate.

[0035] In the alkyl (meth)acrylate having a linear or branched alkyl group having 1 to 8 or more carbon atoms, the alkyl group preferably has 2 to 8 carbon atoms, and more preferably 4 to 8 carbon atoms.

[0036] The proportion of the (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 1 to 8 carbon atoms in all monomer components constituting the acrylic polymer of the present invention is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, still more preferably 60% by mass or more, and particularly preferably 70% by mass or more, relative to the total amount (100% by mass) of all monomer components. Furthermore, from the viewpoint of copolymerizing other monomer components and obtaining the effects of those other monomer components, the proportion may be 99% by mass or less, 96% by mass or less, or 93% by mass or less.

[0037] The acrylic polymer of the present invention is preferably a polymer containing the largest amount of structural units derived from (meth)acrylic acid esters by mass. Examples of the (meth)acrylic acid ester include hydrocarbon group-containing (meth)acrylic acid esters. Examples of the hydrocarbon group-containing (meth)acrylic acid ester include (meth)acrylic acid alkyl esters having a linear or branched aliphatic hydrocarbon group, (meth)acrylic acid esters having an alicyclic hydrocarbon group such as a (meth)acrylic acid cycloalkyl ester, and (meth)acrylic acid esters having an aromatic hydrocarbon group such as a (meth)acrylic acid aryl ester. The hydrocarbon group-containing (meth)acrylic acid esters may be used singly or in combination of two or more.

[0038] Examples of the (meth)acrylic acid alkyl ester include those exemplified as the (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms, those exemplified as the (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 1 to 8 carbon atoms, nonyl (meth)acrylate, isononyl (meth)acrylate, etc.

[0039] Examples of the (meth)acrylic acid ester having an alicyclic hydrocarbon group include (meth)acrylic acid esters having a monocyclic aliphatic hydrocarbon ring, such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, and cyclooctyl (meth)acrylate; (meth)acrylic acid esters having a bicyclic aliphatic hydrocarbon ring, such as isobornyl (meth)acrylate; and (meth)acrylic acid esters having a tricyclic or higher aliphatic hydrocarbon ring, such as dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, tricyclopentanyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, and 2-ethyl-2-adamantyl (meth)acrylate.

[0040] Examples of the (meth)acrylic acid ester having an aromatic hydrocarbon group include (meth)acrylic acid phenyl ester and (meth)acrylic acid benzyl ester.

[0041] In order to properly exhibit the basic properties such as adhesiveness of the hydrocarbon group-containing (meth)acrylic acid ester in the pressure-sensitive adhesive layer, the proportion of the hydrocarbon group-containing (meth)acrylic acid ester in all monomer components constituting the acrylic polymer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and may be 80% by mass or more, 90% by mass or more, or 95% by mass or more, relative to the total amount (100% by mass) of all monomer components. Furthermore, from the viewpoint of copolymerizing other monomer components and obtaining the effects of the other monomer components, the proportion may be 99.9% by mass or less, or may be 98% by mass or less, 95% by mass or less, or may be 90% by mass or less.

[0042] The acrylic polymer of the present invention may contain structural units derived from other monomer components copolymerizable with the hydrocarbon group-containing (meth)acrylic acid ester for the purpose of improving cohesive strength, introducing crosslinking points, or other modifications. Examples of the other monomer components include polar group-containing monomers such as carboxy group-containing monomers, acid anhydride monomers, hydroxy group-containing monomers, glycidyl group-containing monomers, sulfonic acid group-containing monomers, phosphate group-containing monomers, and nitrogen atom-containing monomers. Only one type of each of the other monomer components may be used, or two or more types may be used.

[0043] Examples of the hydroxy group-containing monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate.

[0044] Examples of the nitrogen atom-containing monomer include amide group-containing monomers, amino group-containing monomers, cyano group-containing monomers, and monomers having a nitrogen atom-containing ring. Examples of the amide group-containing monomer include (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylolpropane(meth)acrylamide, N-methoxymethyl(meth)acrylamide, and N-butoxymethyl(meth)acrylamide. Examples of the amino group-containing monomer include aminoethyl(meth)acrylate, N,N-dimethylaminoethyl(meth)acrylate, and t-butylaminoethyl(meth)acrylate. Examples of the cyano group-containing monomer include acrylonitrile and methacrylonitrile. Examples of the monomer having a nitrogen atom-containing ring include N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-vinylmorpholine, N-vinylcaprolactam, and N-(meth)acryloylmorpholine.

[0045] Examples of the carboxy group-containing monomer include acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, etc. Examples of the acid anhydride monomer include maleic anhydride, itaconic anhydride, etc.

[0046] Examples of the keto group-containing monomer include diacetone (meth)acrylamide, diacetone (meth)acrylate, vinyl methyl ketone, vinyl ethyl ketone, allyl acetoacetate, and vinyl acetoacetate.

[0047] Examples of the alkoxysilyl group-containing monomer include 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane.

[0048] Examples of the glycidyl group-containing monomer include glycidyl (meth)acrylate and methylglycidyl (meth)acrylate.

[0049] Examples of the sulfonic acid group-containing monomer include styrenesulfonic acid, allylsulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid.

[0050] The phosphate group-containing monomer may, for example, be 2-hydroxyethyl acryloyl phosphate.

[0051] The polar group-containing monomer constituting the acrylic polymer of the present invention preferably contains a hydroxy group-containing monomer and / or a nitrogen atom-containing monomer, which adjusts the cohesive strength and polarity of the PSA and improves the adhesiveness at room temperature and at high temperatures.

[0052] When the acrylic polymer of the present invention contains the hydroxy group-containing monomer as a monomer component constituting the polymer, the proportion of the hydroxy group-containing monomer in the total monomer components (100% by mass) is not particularly limited, but is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.5% by mass or more. Furthermore, from the viewpoint of improving adhesiveness under room temperature environments and flexibility under low temperature environments, the proportion of the hydroxy group-containing monomer is preferably 30% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, and may even be 3% by mass or less.

[0053] When the acrylic polymer of the present invention contains the nitrogen atom-containing monomer as a monomer component constituting the polymer, the proportion of the nitrogen atom-containing monomer in the total monomer components (100% by mass) is not particularly limited, but is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.5% by mass or more. From the viewpoint of improving adhesiveness under normal temperature conditions and flexibility under low temperature conditions, the proportion of the nitrogen atom-containing monomer is preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, still more preferably 2% by mass or less, and particularly preferably 1% by mass or less.

[0054] The total proportion of the polar group-containing monomers (particularly the total of the nitrogen atom-containing monomers and the hydroxy group-containing monomers) in the total monomer components (100% by mass) constituting the acrylic polymer of the present invention is not particularly limited, but from the viewpoint of better exerting the effect of using the polar group-containing monomers, it is preferably 0.1% by mass or more, more preferably 1% by mass or more. Furthermore, from the viewpoint of obtaining a pressure-sensitive adhesive layer with appropriate flexibility, the total proportion is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 4% by mass or less, particularly preferably 2% by mass or less.

[0055] The monomer components constituting the acrylic polymer of the present invention may further contain other monomers. Examples of the other monomers include vinyl ester monomers such as vinyl acetate, vinyl propionate, and vinyl laurate; aromatic vinyl compounds such as styrene, substituted styrenes (such as α-methylstyrene), and vinyltoluene; olefin monomers such as ethylene, propylene, isoprene, butadiene, and isobutylene; chlorine-containing monomers such as vinyl chloride and vinylidene chloride; alkoxy group-containing monomers such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; and vinyl ether monomers such as methyl vinyl ether and ethyl vinyl ether. Each of the other monomer components may be used singly or in combination of two or more.

[0056] Examples of the alkoxy group-containing monomer include those in which one or more hydrogen atoms in the hydrocarbon group of the hydrocarbon group-containing (meth)acrylic ester are substituted with an alkoxy group, and examples include hydrocarbon group-containing (meth)acrylic esters having an alkoxy group, such as methoxymethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-methoxybutyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, and ethoxyethoxyethyl (meth)acrylate (ethyl carbitol (meth)acrylate).

[0057] The proportion of the other monomers in the total amount (100% by mass) of all monomer components constituting the acrylic polymer of the present invention may be, for example, 0.05% by mass or more, 0.5% by mass or more, 5% by mass or more, or 10% by mass or more, and may be, for example, 20% by mass or less, 10% by mass or less, or 5% by mass or less, or may be substantially absent.

[0058] The weight average molecular weight (Mw) of the acrylic polymer of the present invention is 10 × 10 4 It is preferable that the ratio is 60×10 or more, and more preferably 60×10 4 More preferably, 100×10 4 or more. The Mw is 10 × 10 4 When the Mw is 500×10 or more, a pressure-sensitive adhesive exhibiting good cohesion is easily obtained. 4 It is preferable that the value is equal to or less than 400×10 4 More preferably, 300×10 4 The Mw is 500×10 or less. 4 When the weight average molecular weight is less than 1000 kJ / mol, it is easy to form a pressure sensitive adhesive that exhibits appropriate fluidity (mobility of polymer chains), and therefore the flex resistance is superior. The weight average molecular weight is measured by gel permeation chromatography (GPC) and calculated in terms of polystyrene.

[0059] The glass transition temperature (Tg) of the acrylic polymer of the present invention is preferably 0°C or lower, preferably -10°C or lower, and more preferably -20°C or lower. When the glass transition temperature is 0°C or lower, even when repeatedly bent in a low-temperature environment, folding or marking at the bent portion and peeling of the pressure-sensitive adhesive sheet are unlikely to occur. The glass transition temperature is preferably -80°C or higher, more preferably -70°C or higher, and even more preferably -66°C or higher.

[0060] The glass transition temperature is a value calculated based on the following formula (X) (Fox formula): 1 / Tg=W1 / Tg1+W2 / Tg2+ ... +Wn / Tgn (X) [In formula (X), Tg is the glass transition temperature (unit: K) of the polymer, Tgi (i = 1, 2, ... n) is the glass transition temperature (unit: K) when monomer i forms a homopolymer, and Wi (i = 1, 2, ... n) is the mass fraction of monomer i in all monomer components.] The above formula (X) is a calculation formula when a polymer is composed of n types of monomer components, i.e., monomer 1, monomer 2, ..., monomer n.

[0061] In this specification, the term "glass transition temperature (Tg) when a homopolymer is formed" (sometimes simply referred to as "Tg of the homopolymer") means the "glass transition temperature (Tg) of a homopolymer of the monomer", and specifically, numerical values ​​are listed in "Polymer Handbook" (3rd Edition, John Wiley & Sons, Inc., 1987). The Tg of a homopolymer of a monomer not described in the above document, other than a monomer having a polyorganosiloxane skeleton, refers to, for example, a value obtained by the following measurement method (see JP 2007-51271 A). That is, a reactor equipped with a thermometer, a stirrer, a nitrogen inlet tube, and a reflux condenser was charged with 100 parts by mass of the monomer, 0.2 parts by mass of 2,2'-azobisisobutyronitrile, and 200 parts by mass of ethyl acetate as a polymerization solvent, and the mixture was stirred for 1 hour while introducing nitrogen gas. After removing oxygen from the polymerization system in this manner, the temperature was raised to 63°C and the reaction was allowed to proceed for 10 hours. The mixture was then cooled to room temperature to obtain a homopolymer solution with a solids concentration of 33% by mass. This homopolymer solution was then cast onto a release liner and dried to prepare a test sample (sheet-like homopolymer) with a thickness of approximately 2 mm. This test sample was then punched into a disk shape with a diameter of 7.9 mm, sandwiched between parallel plates, and measured for viscoelasticity in shear mode at a temperature range of -70 to 150°C and a heating rate of 5°C / min using a viscoelasticity tester (trade name "ARES", manufactured by Rheometrics Co., Ltd.) while applying a shear strain of 1 Hz. The peak top temperature of tan δ was taken as the Tg of the homopolymer.

[0062] The acrylic polymer of the present invention can be obtained by polymerizing a composition containing at least an acrylic monomer. The polymerization method is not particularly limited, but examples thereof include solution polymerization, emulsion polymerization, bulk polymerization, thermal polymerization, and polymerization by active energy ray irradiation (active energy ray polymerization). Among these, bulk polymerization, thermal polymerization, and active energy ray polymerization are preferred in terms of the transparency of the pressure-sensitive adhesive layer, cost, etc. Furthermore, the obtained acrylic polymer may be any of a random copolymer, a block copolymer, a graft copolymer, etc.

[0063] Various common solvents may be used during polymerization of the monomer components. Examples of such solvents include organic solvents such as esters such as ethyl acetate and n-butyl acetate; aromatic hydrocarbons such as toluene and benzene; aliphatic hydrocarbons such as n-hexane and n-heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; and ketones such as methyl ethyl ketone and methyl isobutyl ketone. One or more of the above solvents may be used.

[0064] The polymerization initiator, chain transfer agent, emulsifier, etc. used in the radical polymerization of the monomer components are not particularly limited and can be appropriately selected and used. The weight-average molecular weight of the polymer can be controlled by the amounts of the polymerization initiator and chain transfer agent used and the reaction conditions, and the amounts used are appropriately adjusted depending on the types of these.

[0065] As the polymerization initiator used for polymerizing the monomer components, a thermal polymerization initiator, a photopolymerization initiator (photoinitiator), etc. can be used depending on the type of polymerization reaction. Only one type of the polymerization initiator may be used, or two or more types may be used.

[0066] The thermal polymerization initiator is not particularly limited, but examples thereof include azo polymerization initiators, peroxide polymerization initiators (e.g., persulfates such as dibenzoyl peroxide, tert-butyl permaleate, and potassium persulfate, benzoyl peroxide, and hydrogen peroxide), substituted ethane initiators such as phenyl-substituted ethane, aromatic carbonyl compounds, and redox polymerization initiators. Among these, the azo polymerization initiators disclosed in JP-A-2002-69411 are preferred. Examples of the azo polymerization initiator include 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2-methylpropionate)dimethyl, and 4,4'-azobis-4-cyanovaleric acid. The amount of the thermal polymerization initiator used may be any amount that is normally used, and can be selected, for example, from the range of 0.01 to 5 parts by mass, preferably 0.05 to 3 parts by mass, per 100 parts by mass of the monomer component.

[0067] The photopolymerization initiator is not particularly limited, but examples thereof include benzoin ether-based photopolymerization initiators, acetophenone-based photopolymerization initiators, α-ketol-based photopolymerization initiators, aromatic sulfonyl chloride-based photopolymerization initiators, photoactive oxime-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzyl-based photopolymerization initiators, benzophenone-based photopolymerization initiators, ketal-based photopolymerization initiators, and thioxanthone-based photopolymerization initiators. Other examples include acylphosphine oxide-based photopolymerization initiators and titanocene-based photopolymerization initiators. Examples of the benzoin ether-based photopolymerization initiators include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethan-1-one, and anisole methyl ether. Examples of the acetophenone-based photopolymerization initiator include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 4-phenoxydichloroacetophenone, and 4-(t-butyl)dichloroacetophenone. Examples of the α-ketol-based photopolymerization initiator include 2-methyl-2-hydroxypropiophenone and 1-[4-(2-hydroxyethyl)phenyl]-2-methylpropan-1-one. Examples of the aromatic sulfonyl chloride-based photopolymerization initiator include 2-naphthalenesulfonyl chloride. Examples of the photoactive oxime-based photopolymerization initiator include 1-phenyl-1,1-propanedione-2-(O-ethoxycarbonyl)-oxime. Examples of the benzoin-based photopolymerization initiator include benzoin. Examples of the benzyl-based photopolymerization initiator include benzyl. Examples of the benzophenone-based photopolymerization initiator include benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, polyvinylbenzophenone, α-hydroxycyclohexylphenyl ketone, etc. Examples of the ketal-based photopolymerization initiator include benzyl dimethyl ketal, etc.Examples of the thioxanthone-based photopolymerization initiator include thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone. Examples of the acylphosphine oxide-based photopolymerization initiator include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. Examples of the titanocene-based photopolymerization initiator include bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium. The amount of the photopolymerization initiator used may be a normal amount, and can be selected, for example, from the range of 0.01 to 5 parts by mass, preferably 0.05 to 3 parts by mass, per 100 parts by mass of the monomer component.

[0068] The acrylic polymer of the present invention may contain a structural moiety derived from the crosslinking agent. That is, the acrylic polymer of the present invention may be crosslinked by the crosslinking agent. By using a crosslinking agent, a crosslinked structure is formed in the acrylic polymer in the acrylic pressure-sensitive adhesive layer, and the gel fraction can be controlled. The crosslinking agent may be used alone or in combination of two or more.

[0069] The crosslinking agent is not particularly limited, but examples thereof include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, melamine-based crosslinking agents, peroxide-based crosslinking agents, urea-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, carbodiimide-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, amine-based crosslinking agents, hydrazine-based crosslinking agents, silicone-based crosslinking agents, and silane-based crosslinking agents (silane coupling agents).

[0070] The content of the crosslinking agent is not particularly limited, but is preferably 0.001 to 20 parts by mass, more preferably 0.01 to 15 parts by mass, even more preferably 0.15 to 5 parts by mass, still more preferably 0.1 to 3 parts by mass, and particularly preferably 0.2 to 2 parts by mass, relative to 100 parts by mass of the total amount of the monomer components constituting the acrylic polymer of the present invention.

[0071] The isocyanate crosslinking agent is a compound (a polyfunctional isocyanate compound) having an average of two or more isocyanate groups per molecule. Examples of the isocyanate crosslinking agent include aliphatic polyisocyanates, alicyclic polyisocyanates, and aromatic polyisocyanates.

[0072] Examples of the aliphatic polyisocyanates include 1,2-ethylene diisocyanate; tetramethylene diisocyanates such as 1,2-tetramethylene diisocyanate, 1,3-tetramethylene diisocyanate, and 1,4-tetramethylene diisocyanate; hexamethylene diisocyanates such as 1,2-hexamethylene diisocyanate, 1,3-hexamethylene diisocyanate, 1,4-hexamethylene diisocyanate, 1,5-hexamethylene diisocyanate, 1,6-hexamethylene diisocyanate, and 2,5-hexamethylene diisocyanate; 2-methyl-1,5-pentane diisocyanate, 3-methyl-1,5-pentane diisocyanate, and lysine diisocyanate.

[0073] Examples of the alicyclic polyisocyanates include isophorone diisocyanate; cyclohexyl diisocyanates such as 1,2-cyclohexyl diisocyanate, 1,3-cyclohexyl diisocyanate, and 1,4-cyclohexyl diisocyanate; cyclopentyl diisocyanates such as 1,2-cyclopentyl diisocyanate and 1,3-cyclopentyl diisocyanate; hydrogenated xylylene diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated tetramethylxylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate.

[0074] Examples of the aromatic polyisocyanates include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 4,4'-diphenylether diisocyanate, 2-nitrodiphenyl-4,4'-diisocyanate, 2,2'-diphenylpropane-4,4'-diisocyanate, Examples include 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, 4,4'-diphenylpropane diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, naphthylene-1,4-diisocyanate, naphthylene-1,5-diisocyanate, 3,3'-dimethoxydiphenyl-4,4'-diisocyanate, xylylene-1,4-diisocyanate, and xylylene-1,3-diisocyanate.

[0075] Examples of the isocyanate crosslinking agent include commercially available products such as trimethylolpropane / tolylene diisocyanate adduct (trade name "Coronate L", manufactured by Tosoh Corporation), trimethylolpropane / hexamethylene diisocyanate adduct (trade name "Coronate HL", manufactured by Tosoh Corporation), and trimethylolpropane / xylylene diisocyanate adduct (trade name "Takenate D-110N", manufactured by Mitsui Chemicals, Inc.).

[0076] In addition, in the aqueous dispersion of the modified acrylic polymer prepared by emulsion polymerization, it is not necessary to use an isocyanate-based crosslinking agent, but if necessary, a blocked isocyanate-based crosslinking agent can be used because it easily reacts with water.

[0077] When an isocyanate-based crosslinking agent is used as the crosslinking agent, the content of the isocyanate-based crosslinking agent is not particularly limited, but is preferably 0.01 parts by mass or more, more preferably 0.02 parts by mass or more, relative to 100 parts by mass of the total amount of the monomer components constituting the acrylic polymer of the present invention. The content is preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, even more preferably 0.3 parts by mass or less, even more preferably 0.2 parts by mass or less, and particularly preferably 0.1 parts by mass or less.

[0078] Examples of the epoxy crosslinking agent (polyfunctional epoxy compound) include N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, sorbitol polyglycol Examples of the epoxy crosslinking agent include diglycidyl ether, glycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether, sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl-tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. Examples of the epoxy crosslinking agent include commercially available products such as "Tetrad C" (manufactured by Mitsubishi Gas Chemical Company, Inc.).

[0079] When an epoxy-based crosslinking agent is used as the crosslinking agent, the content of the epoxy-based crosslinking agent is not particularly limited, but is preferably more than 0 part by mass and 1 part by mass or less, more preferably 0.001 to 0.5 parts by mass, still more preferably 0.002 to 0.2 parts by mass, still more preferably 0.005 to 0.1 parts by mass, still more preferably 0.008 to 0.1 parts by mass, and particularly preferably 0.009 to 0.05 parts by mass, relative to 100 parts by mass of the total amount of the monomer components constituting the acrylic polymer of the present invention.

[0080] Any peroxide-based crosslinking agent can be used as long as it generates radical active species by heat and promotes crosslinking of the base polymer. Taking into consideration workability and stability, it is preferable to use a peroxide whose 1-minute half-life temperature is 80 to 160°C, and it is more preferable to use a peroxide whose 1-minute half-life temperature is 90 to 140°C.

[0081] Examples of the peroxide-based crosslinking agent include di(2-ethylhexyl)peroxydicarbonate (1-minute half-life temperature: 90.6°C), di(4-t-butylcyclohexyl)peroxydicarbonate (1-minute half-life temperature: 92.1°C), di-sec-butylperoxydicarbonate (1-minute half-life temperature: 92.4°C), t-butylperoxyneodecanoate (1-minute half-life temperature: 103.5°C), t-hexylperoxypivalate (1-minute half-life temperature: 109.1°C), t-butylperoxypivalate (1-minute half-life temperature: 110.3°C), dilauroylperoxy peroxide (1-minute half-life temperature: 116.4°C), di-n-octanoyl peroxide (1-minute half-life temperature: 117.4°C), 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate (1-minute half-life temperature: 124.3°C), di(4-methylbenzoyl)peroxide (1-minute half-life temperature: 128.2°C), dibenzoyl peroxide (1-minute half-life temperature: 130.0°C), t-butylperoxyisobutyrate (1-minute half-life temperature: 136.1°C), 1,1-di(t-hexylperoxy)cyclohexane (1-minute half-life temperature: 149.2°C), and the like.

[0082] The half-life of the peroxide-based crosslinking agent is an index representing the decomposition rate of the peroxide, and refers to the time until the remaining amount of peroxide is reduced by half. The decomposition temperature required to obtain the half-life at a given time and the half-life time at a given temperature are described in manufacturer catalogs, such as NOF Corporation's "Organic Peroxide Catalog, 9th Edition (May 2003)." The amount of decomposed peroxide remaining after the reaction can be measured, for example, by HPLC (high-performance liquid chromatography). More specifically, for example, approximately 0.2 g of the PSA after the reaction is taken, immersed in 10 ml of ethyl acetate, and shaken at 120 rpm at 25°C for 3 hours in a shaker for extraction, followed by leaving the mixture at room temperature for 3 days. Next, 10 ml of acetonitrile is added, and the mixture is shaken at 120 rpm at 25°C for 30 minutes. Approximately 10 μl of the extract obtained by filtering through a membrane filter (0.45 μm) is injected into HPLC for analysis, and the amount of peroxide after the reaction can be determined.

[0083] When a peroxide-based crosslinking agent is used as the crosslinking agent, the content of the crosslinking agent is not particularly limited, but is preferably 2 parts by mass or less, more preferably 0.02 to 2 parts by mass, still more preferably 0.05 to 1.5 parts by mass, still more preferably 0.05 to 1 part by mass, and particularly preferably 0.1 to 1 part by mass, relative to 100 parts by mass of the total amount of the monomer components constituting the acrylic polymer of the present invention.

[0084] The crosslinking agent may also be an organic crosslinking agent or a polyfunctional metal chelate. Polyfunctional metal chelates are compounds in which a polyvalent metal is covalently or coordinately bonded to an organic compound. Examples of polyvalent metal atoms include Al, Cr, Zr, Co, Cu, Fe, Ni, V, Zn, In, Ca, Mg, Mn, Y, Ce, Sr, Ba, Mo, La, Sn, and Ti. Examples of atoms in the organic compound that form covalent or coordinate bonds include oxygen atoms, and examples of organic compounds include alkyl esters, alcohol compounds, carboxylic acid compounds, ether compounds, and ketone compounds.

[0085] The crosslinking agent preferably contains an isocyanate-based crosslinking agent. It is more preferable to contain another crosslinking agent together with the isocyanate-based crosslinking agent. The other crosslinking agent is preferably a peroxide-based crosslinking agent. By using such a crosslinking agent, the acrylic polymer of the present invention can provide a pressure-sensitive adhesive layer that is thin but has excellent adhesion.

[0086] The pressure-sensitive adhesive layer of the present invention contains a tackifier. By containing the acrylic polymer of the present invention and a tackifier, the pressure-sensitive adhesive layer of the present invention has excellent adhesion to an adherend, is resistant to peeling even in a low-temperature environment even after repeated bending, and has excellent flex resistance. The above tackifiers may be used alone or in combination of two or more.

[0087] Examples of the tackifier include a tackifying resin and an oligomer. The oligomer may be present as an oligomer in the pressure-sensitive adhesive layer of the present invention, or may be present in the acrylic polymer of the present invention as a structural moiety derived from the oligomer. That is, the acrylic polymer of the present invention may have a structural moiety derived from the oligomer.

[0088] Examples of the tackifying resin include phenol-based tackifying resins, terpene-based tackifying resins, rosin-based tackifying resins, hydrocarbon-based tackifying resins, epoxy-based tackifying resins, polyamide-based tackifying resins, elastomer-based tackifying resins, ketone-based tackifying resins, etc. Only one type of the tackifying resins may be used, or two or more types may be used.

[0089] Examples of the phenolic tackifying resin include terpene phenolic resins, hydrogenated terpene phenolic resins, alkylphenolic resins, and rosin phenolic resins. The terpene phenolic resins are polymers containing terpene residues and phenolic residues, such as copolymers of terpenes and phenolic compounds (terpene-phenol copolymer resins) and phenol-modified terpene homopolymers or copolymers. Examples of terpenes constituting the terpene phenolic resins include monoterpenes such as α-pinene, β-pinene, and limonene (d-isomer, l-isomer, d / l-isomer (dipentene)). The hydrogenated terpene phenolic resins are resins having a hydrogenated structure of the terpene phenolic resins. The alkylphenolic resins are resins (oil-based phenolic resins) obtained from alkylphenols and formaldehyde. Examples of the alkylphenolic resins include novolac and resol types. The rosin phenolic resins are phenol-modified rosins or various rosin derivatives described below. The rosin phenol resin can be obtained, for example, by adding phenol to rosins or various rosin derivatives described below in the presence of an acid catalyst and then thermally polymerizing the resulting mixture.

[0090] Examples of the terpene-based tackifying resin include polymers of terpenes (typically monoterpenes) such as α-pinene, β-pinene, d-limonene, l-limonene, and dipentene. The terpene polymer may be a homopolymer of one type of terpene, or a copolymer of two or more types of terpenes. Examples of homopolymers of one type of terpene include α-pinene polymer, β-pinene polymer, and dipentene polymer. The modified terpene-based tackifying resin is a modified terpene resin (modified terpene resin) obtained by modifying the terpene resin. Examples of the modified terpene resin include styrene-modified terpene resin and hydrogenated terpene resin.

[0091] Examples of the rosin-based tackifying resin include rosins and rosin derivative resins. Examples of the rosins include unmodified rosins (raw rosins) such as gum rosin, wood rosin, and tall oil rosin; and modified rosins (hydrogenated rosin, disproportionated rosin, polymerized rosin, and other chemically modified rosins) obtained by modifying these unmodified rosins through hydrogenation, disproportionation, polymerization, or the like. Examples of the rosin derivative resin include derivatives of the rosins. Examples of the rosin derivative resin include rosin esters, such as unmodified rosin esters, which are esters of unmodified rosin and alcohols, and modified rosin esters, which are esters of modified rosin and alcohols; unsaturated fatty acid-modified rosins obtained by modifying rosin esters with unsaturated fatty acids; unsaturated fatty acid-modified rosin esters obtained by modifying rosin esters with unsaturated fatty acids; rosin alcohols obtained by reducing the carboxyl groups of rosins or the various rosin derivatives described above; and metal salts of rosins or the various rosin derivatives described above. Specific examples of the rosin esters include methyl esters, triethylene glycol esters, glycerin esters, and pentaerythritol esters of unmodified or modified rosin.

[0092] Examples of the hydrocarbon tackifying resin include aliphatic hydrocarbon resins, aromatic hydrocarbon resins, aliphatic cyclic hydrocarbon resins, aliphatic / aromatic petroleum resins (styrene-olefin copolymers, etc.), aliphatic / alicyclic petroleum resins, hydrogenated hydrocarbon resins, coumarone resins, and coumarone-indene resins.

[0093] The softening point of the tackifier resin is preferably 160° C. or lower, more preferably 150° C. or lower, and even more preferably 140° C. or lower. When the softening point is low, the elastic modulus can be maintained low even with a small amount of addition, and the flex resistance in a low-temperature environment is further improved. The softening point is, for example, 60° C. or higher, preferably 70° C. or higher.

[0094] The weight-average molecular weight of the oligomer is preferably 2,500 to 10,000, more preferably 3,000 to 8,000. The weight-average molecular weight can be determined in polystyrene equivalent terms by GPC. For example, it can be measured using a high-speed GPC device "HPLC-8120GPC" manufactured by Tosoh Corporation under the following conditions: Column: TSKgel Super HZM-H / HZ4000 / HZ3000 / HZ2000 Solvent: Tetrahydrofuran Flow rate: 0.6 ml / min

[0095] The oligomer is preferably an acrylic oligomer composed of an acrylic monomer as an essential monomer component. Examples of the acrylic monomer that constitutes the acrylic oligomer include those exemplified and explained as the monomer components that constitute the acrylic polymer of the present invention. The acrylic oligomer preferably contains a (meth)acrylic acid ester having an alicyclic hydrocarbon group as a constituent unit. The acrylic monomer contained as the constituent unit may be one type or two or more types.

[0096] The proportion of the (meth)acrylic acid ester having an alicyclic hydrocarbon group in the total amount (100% by mass) of all monomer components constituting the acrylic oligomer is preferably 40% by mass or more, more preferably 50% by mass or more, and even more preferably 55% by mass or more, and is preferably 99% by mass or less, and may be 97% by mass or less.

[0097] In one embodiment, the acrylic oligomer preferably contains a (meth)acrylic acid alkyl ester as a structural unit. The (meth)acrylic acid alkyl ester is preferably methyl methacrylate (MMA). The proportion of the (meth)acrylic acid alkyl ester in all monomer components constituting the acrylic oligomer is preferably 10% by mass or more, more preferably 20% by mass or more. This proportion is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 45% by mass or less. The acrylic oligomer may also contain the copolymerizable monomer as a structural unit.

[0098] In one embodiment, the acrylic oligomer preferably contains a functional group-containing monomer as a constituent unit. The functional group-containing monomer is preferably a polar group-containing monomer, more preferably a carboxy group-containing monomer. The proportion of the functional group-containing monomer in all monomer components constituting the acrylic oligomer is preferably 3% by mass or more, more preferably 4% by mass or more. This proportion is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 8% by mass or less. The acrylic oligomer may also contain the copolymerizable monomer as a constituent unit.

[0099] The oligomer can be obtained by polymerizing a composition containing the monomer components that constitute the oligomer. Examples of such polymerization methods include those exemplified and described above as polymerization methods for acrylic polymers. Among these, bulk polymerization, thermal polymerization, and active energy ray polymerization are preferred. Various common solvents may be used when polymerizing the monomer components. Examples of the solvent include those exemplified and described above as solvents that may be used in the polymerization of acrylic polymers. Only one of the solvents may be used, or two or more may be used. The polymerization initiator, chain transfer agent, emulsifier, etc. used in the radical polymerization of the monomer components are not particularly limited and may be appropriately selected and used.

[0100] The content of the tackifier in the pressure-sensitive adhesive layer of the present invention is not particularly limited, but is, for example, 0.6 parts by mass or more, preferably 2 parts by mass or more, relative to 100 parts by mass of the total amount of the acrylic polymer of the present invention. When the content is 0.6 parts by mass or more, peeling is unlikely to occur even when repeatedly bent in a low-temperature environment. From the viewpoint of unlikely peeling even when repeatedly bent at low temperatures, the content is preferably less than 30 parts by mass, more preferably 25 parts by mass or less.

[0101] The content of the tackifier in the pressure-sensitive adhesive layer of the present invention is not particularly limited, but is preferably more than 0% by mass and not more than 22% by mass, more preferably 1 to 16% by mass, relative to 100% by mass of the total amount of the pressure-sensitive adhesive layer of the present invention. When the content is within the above range, peeling is unlikely to occur even when the pressure-sensitive adhesive layer is repeatedly bent in a low-temperature environment.

[0102] The pressure-sensitive adhesive layer of the present invention may contain a colorant. The colorant may be a pigment or a dye. Examples of colorants include black colorants, cyan colorants, magenta colorants, and yellow colorants. From the viewpoint of superior visibility and design, black colorants are preferred. The pressure-sensitive adhesive layer may contain only one type of colorant, or two or more types of colorants.

[0103] Examples of black colorants include carbon black, carbon nanotubes, graphite, copper oxide, manganese dioxide, azo pigments such as azomethine azo black, aniline black, perylene black, titanium black, cyanine black, activated carbon, ferrite, magnetite, chromium oxide, iron oxide, molybdenum disulfide, complex oxide black pigments, anthraquinone organic black dyes, and azo organic black dyes. Examples of carbon black include furnace black, channel black, acetylene black, thermal black, and lamp black. Examples of black colorants include C.I. Solvent Black 3, 7, 22, 27, 29, 34, 43, and 70; C.I. Direct Black 17, 19, 22, 32, 38, 51, and 71; C.I. Acid Black 1, 2, 24, 26, 31, 48, 52, 107, 109, 110, 119, 154; C.I. Disperse Black 1, 3, 10, 24; C.I. Pigment Black 1, 7, and the like.

[0104] Examples of cyan colorants include C.I. Solvent Blue 25, 36, 60, 70, 93, and 95; C.I. Acid Blue 6 and 45; C.I. Pigment Blue 1, 2, 3, 15, 15:1, 15:2, 15:3, 15:4, 15:5, 15:6, 16, 17, 17:1, 18, 22, 25, 56, 60, 63, 65, and 66; C.I. Bat Blue 4; 60, and C.I. Pigment Green 7.

[0105] Examples of magenta colorants include C.I. Solvent Red 1, 3, 8, 23, 24, 25, 27, 30, 49, 52, 58, 63, 81, 82, 83, 84, 100, 109, 111, 121, and 122; C.I. Disperse Red 9; C.I. Solvent Violet 8, 13, 14, 21, and 27; C.I. Disperse Violet 1; C.I. C.I. Basic Red 1, 2, 9, 12, 13, 14, 15, 17, 18, 22, 23, 24, 27, 29, 32, 34, 35, 36, 37, 38, 39, 40; C.I. Basic Violet 1, 3, 7, 10, 14, 15, 21, 25, 26, 27, 28, etc. Examples of magenta colorants include, for example, C.I. Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 39, 40, 41, 42, 48:1, 48:2, 48:3, 48:4, 49, 49:1, 50, 51, 52, 52:2, 53:1, 54, 55, 56, 57:1, 58, 60, 60:1, 63, 63:1, 63:2, 64, 64:1, 6 C.I.7, 68, 81, 83, 87, 88, 89, 90, 92, 101, 104, 105, 106, 108, 112, 114, 122, 123, 139, 144, 146, 147, 149, 150, 151, 163, 166, 168, 170, 171, 172, 175, 176, 177, 178, 179, 184, 185, 187, 190, 193, 202, 206, 207, 209, 219, 222, 224, 238, 245; C.I. Pigment Violet 3, 9, 19, 23, 31, 32, 33, 36, 38, 43, and 50; C.I. Bat Red 1, 2, 10, 13, 15, 23, 29, and 35.

[0106] Examples of yellow colorants include C.I. Solvent Yellow 19, 44, 77, 79, 81, 82, 93, 98, 103, 104, 112, and 162; C.I. Pigment Orange 31 and 43; C.I. Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 24, 34, 35, 37, 42, 53, 55, 65, 73, 74, 75, 81, 83, 93, 94, 95, 97, 98, and 100, C.I. Bat Yellow 1, 3, 20, and the like.

[0107] The pressure-sensitive adhesive layer of the present invention may further contain, as necessary, additives such as crosslinking accelerators, antioxidants, antioxidants, plasticizers, softeners, surfactants, antistatic agents, surface lubricants, leveling agents, light stabilizers, UV absorbers, polymerization inhibitors, foil-like materials, and rust inhibitors, within the range that does not impair the effects of the present invention. Only one of the above additives may be used, or two or more of them may be used.

[0108] The rust inhibitor is a compound that prevents metal rust and corrosion. When the adherend is metal, rust and corrosion can be inhibited when the pressure-sensitive adhesive sheet is attached. Examples of the rust inhibitor include amine compounds, benzotriazole compounds, and nitrites. Other examples include ammonium benzoate, ammonium phthalate, ammonium stearate, ammonium palmitate, ammonium oleate, ammonium carbonate, dicyclohexylamine benzoate, urea, urotropine, thiourea, phenyl carbamate, and cyclohexylammonium-N-cyclohexylcarbamate (CHC). One type of rust inhibitor may be used alone, or two or more types may be used.

[0109] The content of the rust inhibitor is not particularly limited, but is preferably 0.02 to 15 parts by mass per 100 parts by mass of the base polymer. When the content is 0.02 parts by mass or more, good corrosion prevention performance is easily obtained. When the content is 15 parts by mass or less, transparency is easily ensured.

[0110] Among these, benzotriazole-based compounds are preferred as the rust inhibitors, since they can achieve a well-balanced and high level of compatibility with the base polymer, adhesive reliability, transparency, and corrosion prevention properties, and can also achieve excellent appearance.

[0111] The content of the benzotriazole-based compound is not particularly limited, but is preferably 0.02 to 3 parts by mass, more preferably 0.02 to 2.5 parts by mass, and even more preferably 0.02 to 2 parts by mass, per 100 parts by mass of the base polymer.

[0112] The thickness of the pressure-sensitive adhesive layer of the present invention is preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 30 μm or less. When the thickness is 50 μm or less, the difference between the inner and outer diameters when bent is small, and stress applied when bent is easily alleviated. The thickness is not particularly limited, but from the viewpoint of excellent adhesiveness and resistance to peeling when bent, it is preferably 6 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more.

[0113] When the pressure-sensitive adhesive sheet of the present invention is a double-sided pressure-sensitive adhesive sheet with a substrate, the total thickness of the pressure-sensitive adhesive layer on one side is not particularly limited, but is preferably 6 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more. A thickness of 6 μm or more provides excellent adhesion and is less likely to peel when bent. The total thickness of the pressure-sensitive adhesive layer on one side is preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 30 μm or less. A thickness of 50 μm or less reduces the difference between the inner and outer diameters when bent, making it easier to alleviate stress applied when bent. When the pressure-sensitive adhesive sheet is a double-sided pressure-sensitive adhesive sheet with a substrate, the thicknesses of the pressure-sensitive adhesive layers on both sides may be the same or different.

[0114] The pressure-sensitive adhesive layer constituting the pressure-sensitive adhesive sheet of the present invention may be in any form, for example, an emulsion type, a solvent type (solution type), an active energy ray curable type, a hot melt type (hot melt type), etc. Among these, a solvent type or an active energy ray curable type pressure-sensitive adhesive layer is preferred because it is easy to obtain a pressure-sensitive adhesive layer with excellent productivity.

[0115] Examples of the active energy rays include ionizing radiation such as α rays, β rays, γ rays, neutron rays, and electron beams, as well as ultraviolet rays, and ultraviolet rays are particularly preferred. That is, the active energy ray-curable pressure-sensitive adhesive layer is preferably an ultraviolet-curable pressure-sensitive adhesive layer.

[0116] The pressure-sensitive adhesive layer can be produced, for example, by applying (coating) a pressure-sensitive adhesive composition for forming the pressure-sensitive adhesive layer onto a release liner and drying and curing the resulting pressure-sensitive adhesive composition layer, or by applying (coating) the pressure-sensitive adhesive composition onto a release liner and irradiating the resulting pressure-sensitive adhesive composition layer with active energy rays to cure it. If necessary, the resulting pressure-sensitive adhesive layer may be further dried by heating.

[0117] (Substrate) The substrate is an element that functions as a support in the pressure-sensitive adhesive sheet. The substrate may be a single layer, or may be a laminate of substrates of the same or different types.

[0118] Examples of the substrate include plastic substrates (e.g., plastic films), porous materials such as paper, cloth, and nonwoven fabric, nets, and foam sheets. Plastic substrates (particularly plastic films) are preferred. Furthermore, the substrate is preferably a non-foam sheet.

[0119] Examples of resins constituting the plastic substrate include polyolefin resins such as low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, high-density polyethylene, very low-density polyethylene, random copolymer polypropylene, block copolymer polypropylene, homopolypropylene, polybutene, polymethylpentene, ethylene-vinyl acetate copolymer (EVA), ionomer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester (random, alternating) copolymer, ethylene-butene copolymer, and ethylene-hexene copolymer; polyurethane resins; rubber resins (natural rubber, synthetic rubber, mixtures thereof, etc.); polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate, and polybutylene terephthalate (PBT); polycarbonate; polyimide; polyether ether ketone; polyetherimide; polyamides such as aramid and wholly aromatic polyamide; polyphenyl sulfide; fluororesin; polyvinyl chloride; polyvinylidene chloride; cellulose resin; and silicone resin. Only one of the above resins may be used, or two or more may be used.

[0120] The substrate may contain various additives such as fillers (inorganic fillers, organic fillers, etc.), colorants (pigments or dyes), dispersants (surfactants, etc.), antioxidants, antioxidants, UV absorbers, antistatic agents, lubricants, plasticizers, etc. The blending ratio of the various additives is about less than 30% by mass (for example, less than 20% by mass, typically less than 10% by mass) relative to 100% by mass of the total mass of the substrate.

[0121] The substrate may include an auxiliary layer, such as a colored layer, a reflective layer, an undercoat layer, or an antistatic layer, provided on the surface of the substrate.

[0122] The surface of the substrate may be subjected to surface treatments such as physical treatments such as corona discharge treatment, plasma treatment, sand matting treatment, ozone exposure treatment, flame exposure treatment, high-voltage shock exposure treatment, and ionizing radiation treatment; chemical treatments such as chromic acid treatment; and adhesion-enhancing treatments using a coating agent (primer), for the purpose of improving adhesion and retention with the pressure-sensitive adhesive layer. The surface treatment for improving adhesion is preferably applied to the entire surface of the substrate.

[0123] (Adhesive Sheet) The thickness of the adhesive sheet is preferably 6 to 100 μm, more preferably 100 to 80 μm, and even more preferably 20 to 70 μm. When the thickness is 6 μm or more, the adhesiveness is excellent and peeling is less likely to occur when the sheet is bent. When the thickness is 100 μm or less, the difference between the inner and outer diameters when the sheet is bent is small, making it easier to alleviate the stress applied when the sheet is bent. Note that the thickness of the adhesive sheet refers to the thickness from the surface of the substrate on which no adhesive layer is formed to the adhesive surface in the case of a single-sided adhesive sheet, or the thickness from one adhesive surface to the other adhesive surface in the case of a double-sided adhesive sheet, i.e., the thickness of the adhesive body, and does not include the release liner.

[0124] The pressure-sensitive adhesive sheet of the present invention may have a release liner attached to the surface (adhesive surface) of the pressure-sensitive adhesive layer until use. When the pressure-sensitive adhesive sheet is a double-sided pressure-sensitive adhesive sheet, each of the adhesive surfaces on both sides of the pressure-sensitive adhesive sheet may be protected by two release liners, or may be protected by a single release liner with release surfaces on both sides in a rolled form (rolled body). The release liner is used as a protective material for the pressure-sensitive adhesive layer and is peeled off when the sheet is attached to an adherend. However, the release liner is not necessarily provided.

[0125] The release liner can be a conventional release paper, and is not particularly limited. Examples include substrates with a release treatment layer, low-adhesion substrates made of fluoropolymers, and low-adhesion substrates made of non-polar polymers. Examples of substrates with a release treatment layer include plastic films and papers surface-treated with release agents such as silicone-based, long-chain alkyl-based, fluorine-based, and molybdenum sulfide-based release agents. Examples of fluorine-based polymers in the low-adhesion substrates made of fluoropolymers include polytetrafluoroethylene, polychlorotrifluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, tetrafluoroethylene-hexafluoropropylene copolymers, and chlorofluoroethylene-vinylidene fluoride copolymers. Examples of non-polar polymers include olefin-based resins (e.g., polyethylene, polypropylene, etc.). The release liner can be formed by known or conventional methods. The thickness of the release liner is also not particularly limited.

[0126] The pressure-sensitive adhesive sheet is preferably for attaching electrical and electronic components, that is, for use by being attached to components included in electrical and electronic devices. The pressure-sensitive adhesive sheet is particularly preferably used for applications in which components included in electrical and electronic devices are attached to each of the two adhesive surfaces of the double-sided pressure-sensitive adhesive sheet, i.e., for fixing components together in electrical and electronic devices. The double-sided pressure-sensitive adhesive sheet may be used for either fixing or temporarily fixing the components together.

[0127] The term "electrical and electronic devices" refers to devices that fall into at least either an electrical device or an electronic device. Examples of the electrical and electronic devices include image display devices such as liquid crystal displays, electroluminescent displays, and plasma displays, as well as portable electronic devices.

[0128] Examples of the portable electronic device include mobile phones, smartphones, tablet computers, notebook computers, various wearable devices (for example, wristwear devices worn on the wrist like a wristwatch, modular devices worn on a part of the body with a clip or strap, eyewear devices including eyeglasses (monocular and binocular, including head-mounted devices), clothing devices attached to shirts, socks, hats, etc. as accessories, and earwear devices attached to the ears like earphones), digital cameras, digital video cameras, audio equipment (portable music players, IC recorders, etc.), calculators (calculators, etc.), portable game devices, electronic dictionaries, electronic organizers, e-books, in-car information devices, portable radios, portable televisions, portable printers, portable scanners, and portable modems. In this specification, "portable" does not simply mean being portable, but also means having a level of portability that allows an individual (average adult) to carry it relatively easily. The double-sided PSA sheet is used, for example, so that the PSA layer adheres to components of the portable electronic device.

[0129] The pressure-sensitive adhesive sheet of the present invention has excellent flex resistance in low-temperature environments. Therefore, even when used in a location where repeated bending occurs in a low-temperature environment, the bent location is unlikely to be broken or marked, and the pressure-sensitive adhesive sheet is unlikely to peel off. Furthermore, the pressure-sensitive adhesive sheet of the present invention has excellent adhesion to an adherend in room temperature and high-temperature environments. Therefore, the pressure-sensitive adhesive sheet of the present invention is preferably used in a location where the sheet is repeatedly folded. Therefore, the pressure-sensitive adhesive sheet of the present invention is preferably used for bonding components (particularly between components) in electrical and electronic devices that are used while being folded, such as electrical and electronic devices having a foldable image display device (flexible display) (particularly a foldable image display device (foldable display)).

[0130] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.

[0131] Preparation Example 1 (Preparation of Acrylic Polymer A) A reaction vessel equipped with a stirrer, thermometer, nitrogen gas inlet tube, reflux condenser, and dropping funnel was charged with 70 parts by weight of 2-ethylhexyl acrylate (2EHA), 20 parts by weight of n-butyl acrylate (BA), 8 parts by weight of lauryl acrylate (LA), 1 part by weight of 4-hydroxybutyl acrylate (4HBA), and 0.6 parts by weight of N-vinyl-2-pyrrolidone (NVP) as monomer components, 0.1 parts by weight of 2,2'-azobisisobutyronitrile (AIBN) as a thermal polymerization initiator, and a mixture (solids concentration 47% by weight) containing ethyl acetate as a polymerization solvent, and the mixture was stirred at 56°C for 6 hours under a nitrogen atmosphere (polymerization reaction). This resulted in a polymer solution containing acrylic polymer A. The weight-average molecular weight of the acrylic polymer A in this polymer solution was approximately 2,000,000, and the glass transition temperature was -63°C.

[0132] Preparation Example 2 (Preparation of Acrylic Polymer B) In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen gas inlet tube, a reflux condenser, and a dropping funnel, 95 parts by mass of 2EHA and 5 parts by mass of AA as monomer components and 199 parts by mass of ethyl acetate as a polymerization solvent were charged, and the mixture was stirred for 2 hours while introducing nitrogen gas. After removing oxygen from the polymerization system in this way, 0.2 parts by mass of benzoyl peroxide was added as a polymerization initiator, and the mixture was solution polymerized at 60 ° C for 6 hours to obtain a solution of acrylic polymer B. The Mw of this acrylic polymer B was about 120 × 10 4 It was.

[0133] Preparation Example 3 (Preparation of Oligomer A) 60 parts by mass of dicyclopentanyl methacrylate and 40 parts by mass of methacrylic acid as monomer components, 3.5 parts by mass of α-thioglycerol as a chain transfer agent, and 100 parts by mass of toluene as a polymerization solvent were mixed and stirred at 70°C for 1 hour under a nitrogen atmosphere. Next, 0.2 parts by mass of AIBN was added as a thermal polymerization initiator, and the mixture was reacted at 70°C for 2 hours, then heated to 80°C and reacted for 2 hours. Thereafter, the reaction solution was heated to 130°C, and the toluene, chain transfer agent, and unreacted monomer were dried and removed to obtain a solid acrylic oligomer (oligomer A). The weight average molecular weight of oligomer A was 5,100.

[0134] Preparation Example 4 (Preparation of Oligomer B) 95 parts by mass of cyclohexyl methacrylate as monomer components, 5 parts by mass of AA, 10 parts by mass of α-methylstyrene dimer as a chain transfer agent, 10 parts by mass of AIBN as a polymerization initiator, and 120 parts by mass of toluene as a polymerization solvent were mixed and reacted at 85°C for 5 hours under a nitrogen atmosphere to obtain a solution of Oligomer B with a solids concentration of 50% by mass. The weight average molecular weight of Oligomer B was 4,300.

[0135] Example 1 (Preparation of adhesive composition) To the solution of acrylic polymer A prepared in Preparation Example 1, 3 parts by mass of oligomer A prepared in Preparation Example 3 as a tackifier, 0.26 parts by mass of dibenzoyl peroxide (trade name "Niper BMT-40SV", manufactured by NOF Corporation) as crosslinking agent A, and 0.03 parts by mass of an isocyanate crosslinking agent (trade name "Coronate L", manufactured by Tosoh Corporation) as crosslinking agent B were added per 100 parts by mass of acrylic polymer A, and the mixture was stirred and mixed to prepare an adhesive composition.

[0136] (Preparation of Pressure-Sensitive Adhesive Sheet) The pressure-sensitive adhesive composition was applied to a release-treated layer of a 75 μm-thick polyethylene terephthalate film (product name "Diafoil MRF", manufactured by Mitsubishi Chemical Corporation) one side of which had been release-treated with silicone, so that the thickness of the pressure-sensitive adhesive layer was 25 μm, and the applied composition was dried at 150° C. for 3 minutes to form a pressure-sensitive adhesive layer. A release-treated layer of a 38 μm-thick polyethylene terephthalate film (product name "Diafoil MRF", manufactured by Mitsubishi Chemical Corporation) one side of which had been release-treated with silicone was then superimposed on the pressure-sensitive adhesive layer, to prepare the double-sided pressure-sensitive adhesive sheet of Example 1.

[0137] Example 2 (Preparation of adhesive composition) To the solution of acrylic polymer A prepared in Preparation Example 1, 6 parts by mass of oligomer A prepared in Preparation Example 3 as a tackifier, 0.52 parts by mass of dibenzoyl peroxide (trade name "Niper BMT-40SV", manufactured by NOF Corporation) as crosslinking agent A, and 0.05 parts by mass of an isocyanate crosslinking agent (trade name "Coronate L", manufactured by Tosoh Corporation) as crosslinking agent B were added per 100 parts by mass of acrylic polymer A, and the mixture was stirred and mixed to prepare an adhesive composition.

[0138] (Preparation of Pressure-Sensitive Adhesive Sheet) A double-sided pressure-sensitive adhesive sheet of Example 2 was prepared in the same manner as in Example 1, except that the above-described pressure-sensitive adhesive composition was used.

[0139] Example 3 A pressure-sensitive adhesive composition and a double-sided pressure-sensitive adhesive sheet were prepared in the same manner as in Example 2, except that 20 parts by mass of Oligomer B prepared in Preparation Example 4 was used as the tackifier.

[0140] Example 4 A pressure-sensitive adhesive composition and a double-sided pressure-sensitive adhesive sheet were prepared in the same manner as in Example 2, except that 6 parts by mass of Oligomer A and 6 parts by mass of Oligomer B were used as tackifiers.

[0141] Example 5 A pressure-sensitive adhesive composition and a double-sided pressure-sensitive adhesive sheet were prepared in the same manner as in Example 2, except that 6 parts by mass of Oligomer A and 15 parts by mass of Oligomer B were used as tackifiers.

[0142] Example 6 A PSA composition and a double-sided PSA sheet were prepared in the same manner as in Example 2, except that 20 parts by mass of tackifier resin B (trade name "PENSEL D-125", rosin ester, manufactured by Arakawa Chemical Industries, Ltd., softening point approximately 125°C) was used as the tackifier.

[0143] Example 7 A pressure-sensitive adhesive composition and a double-sided pressure-sensitive adhesive sheet were prepared in the same manner as in Example 2, except that 10 parts by mass of oligomer A and 10 parts by mass of tackifying resin A (trade name "YS Polystar S145", terpene phenol resin, manufactured by Yasuhara Chemical Co., Ltd., softening point approximately 145°C) were used as the tackifier.

[0144] Example 8 (Preparation of Pressure-Sensitive Adhesive Composition) To the solution of acrylic polymer A prepared in Preparation Example 1, 10 parts by mass of oligomer B as a tackifier and 0.2 parts by mass of an isocyanate-based crosslinking agent (trade name "Coronate L", manufactured by Tosoh Corporation) as crosslinking agent B were added relative to 100 parts by mass of acrylic polymer A, and the mixture was stirred and mixed to prepare a pressure-sensitive adhesive composition.

[0145] (Preparation of Pressure-Sensitive Adhesive Sheet) A double-sided pressure-sensitive adhesive sheet of Example 8 was prepared in the same manner as in Example 1, except that the above pressure-sensitive adhesive composition was used.

[0146] Comparative Example 1 A pressure-sensitive adhesive composition and a double-sided pressure-sensitive adhesive sheet were prepared in the same manner as in Example 1, except that no tackifier was added.

[0147] Comparative Example 2 (Preparation of Pressure-Sensitive Adhesive Composition) To the solution of acrylic polymer A prepared in Preparation Example 1, 30 parts by mass of tackifier resin B (trade name "Pensel D-125", rosin ester, manufactured by Arakawa Chemical Industries, Ltd., softening point approximately 125°C) as a tackifier, 0.78 parts by mass of dibenzoyl peroxide (trade name "Niper BMT-40SV", manufactured by NOF Corporation) as crosslinking agent A, and 0.1 parts by mass of an isocyanate crosslinking agent (trade name "Coronate L", manufactured by Tosoh Corporation) as crosslinking agent B were added per 100 parts by mass of acrylic polymer A, and the mixture was stirred and mixed to prepare a pressure-sensitive adhesive composition.

[0148] (Preparation of Pressure-Sensitive Adhesive Sheet) A double-sided pressure-sensitive adhesive sheet of Comparative Example 2 was prepared in the same manner as in Example 1, except that the above pressure-sensitive adhesive composition was used.

[0149] Comparative Example 3 (Preparation of Pressure-Sensitive Adhesive Composition) To the solution of acrylic polymer B prepared in Preparation Example 2, 10 parts by mass of tackifier resin A (trade name "YS Polystar S145", terpene phenol resin, manufactured by Yasuhara Chemical Co., Ltd., softening point approximately 145°C) as a tackifier, 3 parts by mass of an isocyanate-based crosslinking agent (trade name "Coronate L", manufactured by Tosoh Corporation) as crosslinking agent B, and 0.03 parts by mass of an epoxy-based crosslinking agent (trade name "TETRAD-C", manufactured by Mitsubishi Gas Chemical Company, Inc.) as crosslinking agent C were added per 100 parts by mass of acrylic polymer B, and the mixture was stirred and mixed to prepare a pressure-sensitive adhesive composition.

[0150] (Preparation of Pressure-Sensitive Adhesive Sheet) The pressure-sensitive adhesive composition was applied to a release-treated layer of a 75 μm-thick polyethylene terephthalate film (product name "Diafoil MRF", manufactured by Mitsubishi Chemical Corporation) one side of which had been release-treated with silicone, so that the thickness of the pressure-sensitive adhesive layer was 25 μm, and the applied composition was dried at 100° C. for 2 minutes to form a pressure-sensitive adhesive layer. A release-treated layer of a 38 μm-thick polyethylene terephthalate film (product name "Diafoil MRF", manufactured by Mitsubishi Chemical Corporation) one side of which had been release-treated with silicone was then superimposed on the pressure-sensitive adhesive layer, to prepare a double-sided pressure-sensitive adhesive sheet of Example 1.

[0151] Comparative Example 4 (Preparation of Pressure-Sensitive Adhesive Composition) To the solution of acrylic polymer A prepared in Preparation Example 1, 20 parts by mass of tackifier resin B (trade name "Pensel D-125", rosin ester, manufactured by Arakawa Chemical Industries, Ltd., softening point approximately 125°C) as a tackifier, 0.26 parts by mass of dibenzoyl peroxide (trade name "Niper BMT-40SV", manufactured by NOF Corporation) as crosslinking agent A, and 0.05 parts by mass of an isocyanate crosslinking agent (trade name "Coronate L", manufactured by Tosoh Corporation) as crosslinking agent B were added per 100 parts by mass of acrylic polymer A, and the mixture was stirred and mixed to prepare a pressure-sensitive adhesive composition.

[0152] (Preparation of Pressure-Sensitive Adhesive Sheet) A double-sided pressure-sensitive adhesive sheet of Comparative Example 4 was prepared in the same manner as in Example 1, except that the above pressure-sensitive adhesive composition was used.

[0153] <Evaluation> The pressure-sensitive adhesive sheets obtained in the examples and comparative examples were evaluated as follows, and the results are shown in the table.

[0154] (1) Storage Modulus G' (-30°C) The release liners on both sides of the double-sided PSA sheets produced in the Examples and Comparative Examples were peeled off, and the double-sided PSA sheets were laminated to produce test samples with a thickness of approximately 1 mm. These test samples were punched out into disks with a diameter of 7.9 mm, sandwiched between parallel plates, and the viscoelasticity was measured in shear mode at a temperature range of -50 to 150°C and a heating rate of 5°C / min using a viscoelasticity tester (product name "ARES", manufactured by Rheometrics Corporation) while applying a shear strain at a frequency of 1 Hz, and the peak-top strength of G' (dynamic shear storage modulus) at -30°C was determined.

[0155] (2) Gel Fraction Approximately 0.2 g of adhesive was scraped off from the adhesive sheet and wrapped in a porous polytetrafluoroethylene membrane (trade name "NTF-1122", manufactured by Nitto Denko Corporation) with a pore diameter of 0.2 μm cut into a size of 100 mm x 100 mm, and the opening of the wrap was tied with a string. The mass of the adhesive sample (B) was calculated by subtracting the total mass (A) of the porous polytetrafluoroethylene membrane and the string, which had been measured in advance, from the mass of this sample. The adhesive sample wrapped in the porous polytetrafluoroethylene membrane was immersed in approximately 50 mL of ethyl acetate at 23 ° C. for 7 days, and the sol component of the adhesive was eluted out of the porous polytetrafluoroethylene membrane. After immersion, the adhesive wrapped in the porous polytetrafluoroethylene membrane was removed, dried at 130 ° C. for 2 hours, and allowed to cool for approximately 20 minutes, and the dry mass (C) was measured. The gel fraction of the adhesive was calculated using the following formula. Gel fraction (%) = 100 × (C - A) / B

[0156] (3) 180° Peel Adhesion (RT) Under a measurement environment of 23°C and 50% RH, the release liners on both sides of the double-sided PSA sheets prepared in the Examples and Comparative Examples were peeled off, and a 25 μm thick PET film was attached to one adhesive surface of the double-sided PSA sheet to form a backing. A measurement sample was then cut to a size of 20 mm wide and 100 mm long. For each measurement sample prepared, the exposed adhesive surface of the measurement sample was pressed against the surface of a stainless steel plate (SUS304BA plate) using a 2 kg roller, with one reciprocating motion. After leaving this sample in the same environment for 24 hours, the 180° peel strength (adhesive strength) [N / 20 mm] was measured using a universal tension and compression tester under the following conditions: a tensile speed of 300 mm / min, a peel angle of 180°, a temperature of 23°C, and a relative humidity of 50% RH (room temperature). The universal tension and compression tester used was a tension and compression tester (product name "TG-1kN") manufactured by Minebea Co., Ltd. In the case of a single-sided PSA sheet, the PET film backing is not necessary.

[0157] (4) Flexibility Test One release liner was peeled from the double-sided PSA sheets prepared in the Examples and Comparative Examples under an environment of -30°C / 50% RH, and the exposed adhesive surface was bonded to one side of a polyethylene terephthalate film (thickness: 50 μm, Young's modulus: 4.5 GPa). The other release liner was then peeled off, and the exposed adhesive surface was bonded to one side of another polyethylene terephthalate film (thickness: 50 μm, Young's modulus: 4.5 GPa). The sheets were then pressurized at 0.5 MPa and 50°C for 20 minutes in an autoclave manufactured by Kurihara Seisakusho Co., Ltd., and then left for 24 hours under conditions of 23°C and 50% RH. The laminates thus obtained, consisting of [PET film / double-sided PSA sheet / PET film], were cut into 20 mm wide and 200 mm long samples. The obtained sample was repeatedly bent under the following conditions using a durability tester (product name "Planar Body No-Load U-Shaped Stretch Environmental Tester CL09-TypeD01-FSC90", manufactured by Yuasa System Co., Ltd.). Thereafter, after the test at -30°C / 50% RH, the presence or absence of creases in the bent portion of the sample (flex resistance (low temperature)) was visually confirmed, and the flex resistance was evaluated according to the following criteria. <Test conditions> Bending radius: 2 mm, number of flexes: 200,000 times, flex speed: 60 times / min <Evaluation criteria> ◯: No creases or slight creases occurred, but the creases were at a level that was practically usable. △: Bending marks were observed that were visible when held up to a light, but the creases were at a level that was practically usable. ×: Bending occurred to a level that was not practically usable.

[0158] (5) High-Temperature Holding Power In a measurement environment of 23°C and 50% RH, the double-sided PSA sheets prepared in the Examples and Comparative Examples were cut into 10 mm x 20 mm pieces, taking care to prevent adhesive extrusion. The release liner on the light release side (a 38 μm-thick polyethylene terephthalate film with one side treated with silicone for release) was peeled off, and a 25 μm-thick PET film was attached as a backing. The release liner on the heavy release side was then peeled off and attached to a stainless steel plate (SUS304BA plate). A 2 kg roller was then reciprocated at a speed of 5 mm / sec to press the sheet together, and the sheet was left in an 80°C atmosphere for 30 minutes. The sheet was then removed from the measurement environment of 23°C and 50% RH, and the distance of the shift between the PET film and the stainless steel plate (SUS304BA plate) from the starting point was measured. The high-temperature holding power was then evaluated according to the following evaluation criteria. <Evaluation Criteria> ◯: No peeling occurred ×: Peeling occurred

[0159]

[0160] Variations of the invention according to the present disclosure are described below. [Appendix 1] A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer comprising an acrylic polymer containing, as a structural unit, a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms, and a tackifier, the pressure-sensitive adhesive layer having a modulus of elasticity of 5.0 MPa or less and a gel fraction of 50% or more at -30°C. [Appendix 2] The pressure-sensitive adhesive sheet according to Appendix 1, wherein the acrylic polymer contains, as a structural unit, a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 1 to 8 carbon atoms. [Appendix 3] The pressure-sensitive adhesive sheet according to Appendix 1 or 2, wherein the tackifier comprises an oligomer or a tackifier resin. [Appendix 4] The pressure-sensitive adhesive sheet according to any one of Appendix 1 to 3, which is a double-sided pressure-sensitive adhesive sheet for fixing components together in an electrical / electronic device. [Appendix 5] An electrical / electronic device comprising the pressure-sensitive adhesive sheet according to Appendix 4, wherein the pressure-sensitive adhesive sheet fixes components together on both adhesive surfaces.

[0161] 1 double-sided adhesive sheet 2 adhesive layer 3, 4 release liner

Claims

1. An adhesive sheet having an adhesive layer, the adhesive layer comprising an acrylic polymer containing, as a constituent unit, a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 10 or more carbon atoms, and a tackifier, the adhesive layer having an elastic modulus of 5.0 MPa or less at -30°C and a gel fraction of 50% or more.

2. The pressure-sensitive adhesive sheet according to claim 1, wherein the acrylic polymer contains, as a constituent unit, a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 1 to 8 carbon atoms.

3. The pressure-sensitive adhesive sheet according to claim 1 or 2, wherein the tackifier comprises an oligomer or a tackifier resin.

4. The pressure-sensitive adhesive sheet according to claim 1 or 2, which is a double-sided pressure-sensitive adhesive sheet for fixing components together in an electric / electronic device.

5. An electrical / electronic device comprising the adhesive sheet according to claim 4, said adhesive sheet fixing members together with both adhesive surfaces thereof.

Citation Information

Patent Citations

  • Adhesive agent layer for flexible image display device, laminate body for flexible image display device, and flexible image display device

    JP2019218513A

  • Low dielectric constant optically clear adhesives for flexible electronic displays

    JP2020513451A

  • Adhesive sheet rolls and adhesive sheets

    JP7311014B1

  • Pressure-sensitive adhesive layer, pressure-sensitive adhesive sheet using the same, laminate, and flexible image display device

    JP7464194B1

  • Pressure-sensitive adhesive composition

    WO2022220498A1