Laminated sheet for transfer and method for manufacturing same

The transfer laminate sheet with a cholesteric liquid crystal hardening layer and adhesive layer configuration addresses pattern chipping issues, enhancing the clarity and authenticity of display media by reducing chipping and improving visibility.

WO2024203549A1PCT designated stage expired Publication Date: 2024-10-03ZEON CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010585
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing transfer laminate sheets with a liquid crystal hardened layer often suffer from pattern chipping issues, which can obscure the visibility of the pattern and compromise the authenticity identification function of display media.

Method used

A transfer laminate sheet is designed with a configuration that includes a release base layer, an adhesive layer, and a dividing layer with a cholesteric liquid crystal hardening layer, where the adhesive layer is directly connected to the dividing layer and separated by cracks, reducing pattern chipping and improving clarity.

Benefits of technology

The solution effectively reduces pattern chipping and enhances the clarity of the transferred product, making it suitable for applications requiring high recognition and authenticity, such as display media.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010585_03102024_PF_FP_ABST
    Figure JP2024010585_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A laminated sheet for transfer includes, in the following order, a release base material layer, an adhesive layer, and a dividing layer directly contacting the adhesive layer. The dividing layer includes a plurality of small-piece layers that include a cholesteric liquid crystal cured layer and are divided by cracks.
Need to check novelty before this filing date? Find Prior Art

Description

Transfer laminate sheet and its manufacturing method

[0001] The present invention relates to a transfer laminate sheet and a method for producing the same.

[0002] There is known a transfer laminate capable of forming a patterned layer (hereinafter also referred to as a liquid crystal cured layer) obtained by curing a liquid crystal composition containing a polymerizable liquid crystal compound on an adherend (see Patent Documents 1 and 2, etc.). In the techniques of Patent Documents 1 and 2, the liquid crystal cured layer included in the transfer laminate is divided by incisions or cracks.

[0003] International Publication No. WO 2021 / 079815 (corresponding foreign publication: European Patent Application Publication No. 4050387) International Publication No. WO 2021 / 172567 (corresponding foreign publication: European Patent Application Publication No. 4113178)

[0004] When a display medium is formed by transferring a layer including a cured liquid crystal layer to an adherend in a pattern, if there are defects in the pattern of the display medium, the viewer of the display medium may have difficulty or be unable to recognize the pattern. If the pattern displayed on the display medium is difficult to see, the authenticity identification function of the display medium may not be fully demonstrated. Therefore, it is preferable that the pattern of the transfer product obtained by transferring a transfer laminate including a cured liquid crystal layer to an adherend has few defects. When the cured liquid crystal layer included in the transfer laminate is divided, as in the techniques of Patent Documents 1 and 2, defects in the pattern of the transfer product are reduced to a certain extent, but further reduction in defects is required.

[0005] Therefore, there is a need for a laminated sheet for transfer that can reduce pattern chipping in a transferred product containing a cured liquid crystal layer; and a method for producing such a laminated sheet for transfer.

[0006] As a result of intensive research aimed at solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by disposing an adhesive layer between a release substrate layer and a dividing layer including a cured cholesteric liquid crystal layer in a transfer laminate sheet, and have completed the present invention. That is, the present invention provides the following.

[0007] <1> A transfer laminate sheet comprising, in this order, a release base layer, an adhesive layer, and a dividing layer directly adjacent to the adhesive layer, wherein the dividing layer comprises a plurality of small pieces containing a cured cholesteric liquid crystal layer and divided by cracks. <2> The transfer laminate sheet according to <1>, wherein the peel strength between the adhesive layer and the dividing layer is 0.1 N / 25 mm or more and 2 N / 25 mm or less. <3> The transfer laminate sheet according to <1> or <2>, wherein the adhesive layer is provided on the entire surface of the release base layer. <4> The transfer laminate sheet according to any one of <1> to <3>, wherein the transfer laminate sheet is long. <5> The transfer laminate sheet according to any one of <1> to <4>, wherein the adhesive layer is a layer of pressure-sensitive adhesive containing one or more adhesives selected from the group consisting of acrylic pressure-sensitive adhesives, urethane pressure-sensitive adhesives, rubber pressure-sensitive adhesives, silicone pressure-sensitive adhesives, polyester pressure-sensitive adhesives, and ethylene vinyl acetate pressure-sensitive adhesives. <6> The transfer laminate sheet according to any one of <1> to <5>, wherein some or all of the plurality of small fragment layers included in the dividing layer are optical layers including the cured cholesteric liquid crystal layer and a retardation layer. <7> The transfer laminate sheet according to <6>, wherein the retardation layer included in the optical layer is a λ / 4 plate. <8> The transfer laminate sheet according to <6> or <7>, wherein the plurality of small fragment layers included in the dividing layer include two types of optical layers, and the absolute value of the difference between the in-plane retardation values ​​of the two types of optical layers is (λ / 2 - 60 nm) or more (λ / 2 + 60 nm) or less at a measurement wavelength λ. <9> The transfer laminate sheet according to any one of <6> to <8>, wherein the optical layers are arranged in a pattern on the adhesive layer. <10> A method for producing a transfer laminate sheet according to any one of <1> to <9>, comprising: a step (1) of preparing a first laminate including, in this order, the release base layer, the adhesive layer, and a layer (A) directly on the adhesive layer and including the cholesteric liquid crystal cured layer; and a step (2) of forming cracks in the layer (A) included in the first laminate to divide the layer (A) and form a plurality of small fragment layers.

[0008] According to the present invention, it is possible to provide a laminate sheet for transfer, which can reduce chipping of a pattern in a transferred product containing a cured liquid crystal layer, and a method for producing such a laminate sheet for transfer.

[0009] Fig. 1 is a cross-sectional view schematically showing a transfer laminate sheet according to embodiment 1 of the present invention. Fig. 2 is a cross-sectional view schematically showing a transfer laminate sheet according to embodiment 2 of the present invention. Fig. 3 is a cross-sectional view schematically showing a transfer laminate sheet according to embodiment 3 of the present invention.

[0010] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and can be implemented with any modifications within the scope of the claims of the present invention and their equivalents. The components of the embodiments shown below can be combined as appropriate. In addition, in the drawings, the same components are designated by the same reference numerals, and their description may be omitted.

[0011] In the following description, a "long" film refers to a film having a length that is 5 times or more its width, preferably 10 times or more its width, and specifically refers to a film having a length that can be wound into a roll for storage or transportation. There is no particular upper limit to the length of the film, and it can be, for example, 100,000 times or less its width.

[0012] In the following description, unless otherwise specified, the front direction of a certain layer means the normal direction of the principal surface of the layer, and specifically refers to the direction of the polar angle of 0° and the azimuthal angle of 0° of the principal surface.

[0013] In the following description, the term "(meth)acrylic" includes "acrylic", "methacrylic", and combinations thereof. The term "(thio)epoxy" includes "epoxy", "thioepoxy", and combinations thereof. The term "iso(thio)cyanate" includes "isocyanate", "isothiocyanate", and combinations thereof.

[0014] In the following description, unless otherwise specified, the in-plane retardation Re of a layer is a value expressed as Re = (nx - ny) x d. Here, nx represents the refractive index in a direction perpendicular to the thickness direction of the layer (in-plane direction) and giving the maximum refractive index. ny represents the refractive index in the in-plane direction of the layer and perpendicular to the nx direction. nz represents the refractive index in the thickness direction of the layer. d represents the thickness of the layer. The measurement wavelength is 550 nm unless otherwise specified.

[0015] In the following description, unless otherwise specified, the directions of elements as "parallel," "vertical," and "orthogonal" may include an error within a range that does not impair the effects of the present invention, for example, within a range of ±3°, ±2°, or ±1°.

[0016] In the following description, unless otherwise specified, the term "plate" is not limited to rigid members, but also includes flexible members such as resin films.

[0017] In the following description, unless otherwise specified, the peel strength between two given layers is a value measured in accordance with JIS Z0237 at a temperature of 23°C, a peel speed of 300 m / min, and a peel angle of 180°. Peel strength can be measured using a 25 mm x 150 mm test piece cut from the laminate whose peel strength is to be measured. As a measuring device, for example, a "Digital Force Gauge ZP-50" manufactured by IMADA can be used.

[0018] In the following description, unless otherwise specified, the term "adhesive" includes not only adhesives in the narrow sense (adhesives having a shear storage modulus of 1 MPa to 500 MPa at 23° C. after energy ray irradiation or heat treatment) but also pressure-sensitive adhesives (pressure-sensitive adhesives) having a shear storage modulus of less than 1 MPa at 23° C. Therefore, the term "adhesive layer" includes not only a layer of an adhesive in the narrow sense but also a layer of a pressure-sensitive adhesive.

[0019] In the following description, when a surface and a layer are "in direct contact," it means that the surface and layer are in contact with each other and there is no other layer between them, unless otherwise specified. Also, in the following description, when two layers are "in direct contact," it means that the two layers are in contact with each other and there is no other layer between them, unless otherwise specified.

[0020] <1. Transfer Laminate Sheet> <1.1. Overview> A transfer laminate sheet according to one embodiment of the present invention comprises, in this order, a release substrate layer, an adhesive layer, and a dividing layer directly attached to the adhesive layer, the dividing layer comprising a plurality of small fragment layers including a cured cholesteric liquid crystal layer and divided by cracks. Because the transfer laminate sheet has the above-described configuration, pattern chipping is reduced, and a transfer product with improved clarity can be obtained.

[0021] The transfer laminate sheet is preferably long. A long transfer laminate sheet can be produced efficiently.

[0022] <1.2. Release Base Layer> The release base layer is a layer that is peeled off as needed after the transfer laminate sheet is attached to an adherend. Examples of the release base layer are not particularly limited, and plates, sheets, films, etc. formed of appropriate materials can be used. Furthermore, from the viewpoint of efficiently producing the transfer laminate sheet, it is preferable that the release base layer has a long shape.

[0023] Examples of materials for the release substrate layer include resins. Thermoplastic resins are typically used as the resin. The thermoplastic resins may contain a polymer and, if necessary, optional components. Examples of polymers include polycarbonate, polyethersulfone, polyethylene terephthalate, polyimide, polymethyl methacrylate, polysulfone, polyarylate, polyethylene, polyphenylene ether, polystyrene, polyvinyl chloride, cellulose diacetate, cellulose triacetate, and alicyclic structure-containing polymers. An alicyclic structure-containing polymer is a polymer having an alicyclic structure in the main chain and / or side chain. One type of polymer may be used alone, or two or more types may be used in combination in any ratio.

[0024] The release substrate layer may or may not have been subjected to a stretching treatment, and may or may not have been subjected to a surface treatment such as rubbing treatment.

[0025] An adhesive layer is usually provided directly on the release substrate layer. That is, there are usually no other layers between the release substrate layer and the adhesive layer. The peel strength P2 between the release substrate layer and the adhesive layer is preferably greater than the peel strength P1 between the adhesive layer and the dividing layer. This allows the adhesive layer to be peeled from the dividing layer together with the release substrate layer when the release substrate layer is peeled from the transfer laminate sheet. The peel strength P2 between the release substrate layer and the adhesive layer is preferably 8 N / 25 mm or more, more preferably 10 N / 25 mm or more, and preferably 15 N / 25 mm or less, more preferably 12 N / 25 mm or less, provided that P2 > P1.

[0026] The release substrate layer may be a transparent material that transmits light, or may be a non-transparent material that does not transmit light.

[0027] The release substrate layer may have a single layer structure or a multi-layer structure.

[0028] The thickness of the release substrate layer is not particularly limited, but is preferably 5 μm or more, more preferably 10 μm or more, particularly preferably 20 μm or more, and is preferably 1 mm or less, more preferably 500 μm or less, particularly preferably 200 μm or less.

[0029] <1.3. Adhesive Layer> The adhesive layer is provided between the release substrate layer and the dividing layer. By providing the transfer laminate sheet with an adhesive layer, it becomes easy to manufacture a transfer laminate sheet with reduced chipping of the dividing layer, and in a display medium, which is a transferred product obtained by transferring the transfer laminate sheet to a display substrate, chipping of the dividing layer can be reduced, improving the clarity of the display medium. The adhesive layer is preferably provided directly on the release substrate layer.

[0030] (Peel strength between adhesive layer and dividing layer) The peel strength P1 between the adhesive layer and the dividing layer is preferably 0.07 N / 25 mm or more, more preferably 0.1 N / 25 mm or more, even more preferably 0.2 N / 25 mm or more, even more preferably 0.5 N / 25 mm or more, and preferably 3.0 N / 25 mm or less, more preferably 2.0 N / 25 mm or less, even more preferably 1.75 N / 25 mm or less, even more preferably 1.5 N / 25 mm or less. If the peel strength P1 between the adhesive layer and the dividing layer is above the lower limit, the small pieces of the layer that adhere to the processing tool and peel off during the process of forming the dividing layer can be effectively reduced, so that a transfer release sheet with a dividing layer with reduced chipping can be easily produced. In addition, a transfer product with reduced chipping can be produced from the transfer laminate sheet.

[0031] (Material of Adhesive Layer) The adhesive layer is an adhesive layer. Examples of adhesives constituting the adhesive layer include those using various polymers as the base polymer. Examples of such base polymers include acrylic polymers, urethane polymers, rubber polymers, silicone polymers, polyester polymers, ethylene vinyl acetate polymers, and epoxy polymers. The adhesive may also contain optional components such as tackifiers, plasticizers, polymerization initiators, curing agents, UV absorbers, colorants, and antistatic agents in combination with the base polymer. The adhesive layer is preferably an adhesive layer containing one or more adhesives selected from the group consisting of acrylic adhesives, urethane adhesives, rubber adhesives, silicone adhesives, polyester adhesives, and ethylene vinyl acetate adhesives. Here, acrylic adhesives, urethane adhesives, rubber adhesives, silicone adhesives, polyester adhesives, and ethylene vinyl acetate adhesives refer to adhesives whose base polymer is an acrylic polymer, a urethane polymer, a rubber polymer, a silicone polymer, a polyester polymer, and an ethylene vinyl acetate polymer, respectively. An acrylic polymer refers to a polymer whose repeating unit contains (meth)acrylic acid and / or a derivative thereof. A urethane polymer refers to a polymer whose repeating unit contains a urethane structure. A rubber polymer refers to a polymer containing rubber, such as natural rubber or synthetic rubber. A silicone polymer refers to a polymer whose repeating unit contains a siloxane bond. A polyester polymer refers to a polymer whose repeating unit contains a carboxylic acid ester structure. An ethylene vinyl acetate polymer refers to a polymer whose repeating unit contains an ethylene monomer unit and a vinyl acetate monomer unit.

[0032] The adhesive includes a pressure-sensitive adhesive (pressure-sensitive adhesive). The adhesive layer is preferably a layer having sufficient releasability to be peeled off from the dividing layer together with the release base layer when the transfer laminate sheet is transferred to the display substrate and the release base layer is peeled off, and more preferably a pressure-sensitive adhesive layer. Therefore, the adhesive layer is more preferably a layer of pressure-sensitive adhesive containing one or more selected from the group consisting of acrylic pressure-sensitive adhesives, urethane pressure-sensitive adhesives, rubber pressure-sensitive adhesives, silicone pressure-sensitive adhesives, polyester pressure-sensitive adhesives, and ethylene vinyl acetate pressure-sensitive adhesives, and even more preferably a layer of pressure-sensitive adhesive containing one or more selected from the group consisting of acrylic pressure-sensitive adhesives.

[0033] Commercially available adhesive layers may be used, including "PET75-H109," "RB105," "H120," and "RC611" manufactured by Nichiei Shinka Co., Ltd.

[0034] (Thickness of Adhesive Layer) The thickness of the adhesive layer is not particularly limited, and can be, for example, 0.1 μm or more, for example, 0.5 μm or more, for example, 50 μm or less, for example, 30 μm or less.

[0035] (Configuration of adhesive layer, etc.) The adhesive layer may have a single layer structure or a multi-layer structure. In addition, the adhesive layer may or may not have cracks in the thickness direction. Preferably, in a display medium obtained by transferring the transfer laminate sheet to a display substrate, in order to effectively reduce chipping of the dividing layer, the depth of the cracks in the thickness direction is 0 μm (i.e., no cracks), or the depth of the cracks in the thickness direction is deeper than 0 μm and is 1 / 10 or less of the thickness of the adhesive layer.

[0036] Furthermore, the adhesive layer is preferably provided on substantially the entire surface of the release substrate, preferably on the entire surface. In this case, the dividing layer can be adhered to substantially the entire surface, preferably on the entire surface, of the release substrate, making it easier to manufacture the transfer laminate sheet. Furthermore, when transferring the dividing layer in a pattern from the transfer laminate sheet to the display substrate, chipping of the dividing layer can be effectively reduced regardless of which part of the transfer laminate sheet the dividing layer is transferred from. Therefore, the design freedom of the transfer pattern is improved.

[0037] <1.4. Dividing Layer> (Small Piece Layer) The dividing layer includes a plurality of small piece layers. The small piece layers are provided directly on the surface of the adhesive layer so as to cover the surface of the adhesive layer. The plurality of small piece layers are separated from each other by cracks. It is preferable that each of the plurality of small piece layers has the same shape. The shape of each small piece layer as viewed from the thickness direction is not particularly limited. Preferred examples include polygons such as triangles, squares, and hexagons. Among these, equilateral triangles, squares, and regular hexagons are preferred, squares are more preferred, parallelograms are even more preferred, rectangles such as squares and rectangles are even more preferred, and squares are particularly preferred.

[0038] The width of each small piece layer as viewed in the thickness direction is preferably within a specific range. Specifically, the width of the small piece layer is preferably 150 μm or less, more preferably 125 μm or less, even more preferably 100 μm or less, and particularly preferably 80 μm or less. There is no particular lower limit, and it is usually greater than 0 μm, preferably 10 μm or more. The width of the small piece layer refers to the longest distance between multiple parallel lines drawn tangent to the contour of the small piece layer. Such a small width of the small piece layer can make the contour of the display medium obtained by transferring the transfer laminate sheet in a pattern smoother.

[0039] The cracks dividing the plurality of small piece layers may have a shape corresponding to the shape of the small piece layer when viewed in the thickness direction of the small piece layer. For example, if the plurality of small piece layers are square, the cracks may have a lattice shape.

[0040] The depth of the crack is usually greater than or equal to the thickness of the fragment layer, and the crack separates the fracture layer into fragment layers.

[0041] The thickness of the fragment layer is preferably 0.1 μm or more, more preferably 0.5 μm or more, even more preferably 1 μm or more, and is preferably 12 μm or less, more preferably 11 μm or less, even more preferably 10 μm or less. The thicknesses of the fragment layers included in the dividing layer may be different from each other, but are preferably the same.

[0042] The small piece layer includes a cholesteric liquid crystal cured layer. The cholesteric liquid crystal cured layer is a layer having cholesteric regularity and formed by curing a liquid crystal composition containing a polymerizable liquid crystal compound. The cholesteric liquid crystal cured layer may be a layer including multiple types of cholesteric liquid crystal cured layers.

[0043] Cholesteric regularity is a structure in which the molecular axes are aligned in a fixed direction on a certain plane within a material, but the direction of the molecular axes is slightly shifted on the next overlapping plane, and then even more so on the next plane, and so on. As the molecules pass through the successive overlapping planes, the angle of the molecular axes in that plane shifts (twists). That is, when molecules within a layer of a material have cholesteric regularity, the molecules are aligned so that their molecular axes are aligned in a fixed direction on a first plane within the layer. On a second plane within the layer that overlaps the first plane, the direction of the molecular axes is shifted at a slight angle from the direction of the molecular axes on the first plane. On a third plane that overlaps the second plane, the direction of the molecular axes is shifted at an even greater angle from the direction of the molecular axes on the second plane. In this way, the angles of the molecular axes in the overlapping planes are sequentially shifted (twisted). Such a structure in which the direction of the molecular axis is twisted is usually a helical structure, which is an optically chiral structure. A liquid crystal layer containing a liquid crystalline compound having such cholesteric regularity usually reflects circularly polarized light while maintaining its chirality. A liquid crystal layer having cholesteric regularity is generally capable of separating left- and right-handed circularly polarized light. That is, this layer has the property of transmitting one of right-handed and left-handed circularly polarized light and reflecting part or all of the other circularly polarized light.

[0044] The circularly polarized light reflected by the cholesteric liquid crystal cured layer contained in each of the plurality of small fragment layers does not need to have the same rotation direction, but it is preferable that the circularly polarized light has the same rotation direction.

[0045] A cholesteric liquid crystal cured layer can be obtained, for example, by polymerizing a polymerizable liquid crystal compound in a state where it exhibits a cholesteric liquid crystal phase. More specifically, a liquid crystal composition containing a polymerizable liquid crystal compound is applied to a suitable substrate to form a layer, orientated in a cholesteric liquid crystal phase, and cured to obtain a cholesteric liquid crystal cured layer. Hereinafter, a composition in which the polymerizable liquid crystal compound contained in the liquid crystal composition can exhibit a liquid crystal phase having cholesteric regularity (cholesteric liquid crystal phase) when the polymerizable liquid crystal compound is aligned is referred to as a cholesteric liquid crystal composition.

[0046] As the polymerizable liquid crystal compound, a photopolymerizable liquid crystal compound is preferred. As the photopolymerizable liquid crystal compound, a photopolymerizable liquid crystal compound that can be polymerized by irradiation with active energy rays can be used. As the active energy rays, energy rays that can promote the polymerization reaction of the photopolymerizable liquid crystal compound can be adopted from a wide range of energy rays such as visible light, ultraviolet light, and infrared light, but ionizing radiation such as ultraviolet light is particularly preferred. Among them, as the photopolymerizable liquid crystal compound that is suitably used in the cholesteric liquid crystal composition, a rod-shaped liquid crystal compound having two or more reactive groups in one molecule is preferred, and a compound represented by formula (1) is particularly preferred. R 3 -C 3 -D 3 -C 5 -M-C 6 -D 4 -C 4 -R 4 Formula (1)

[0047] In formula (1), R 3 and R 4 are reactive groups, each independently representing a group selected from the group consisting of a (meth)acrylic group, a (thio)epoxy group, an oxetane group, a thietanyl group, an aziridinyl group, a pyrrole group, a vinyl group, an allyl group, a fumarate group, a cinnamoyl group, an oxazoline group, a mercapto group, an iso(thio)cyanate group, an amino group, a hydroxyl group, a carboxyl group, and an alkoxysilyl group. By having these reactive groups, it is possible to obtain a cured liquid crystal composition layer having high mechanical strength when the liquid crystal composition is cured.

[0048] In formula (1), D 3 and D 4 each independently represents a group selected from the group consisting of a single bond, a linear or branched alkyl group having 1 to 20 carbon atoms, and a linear or branched alkylene oxide group having 1 to 20 carbon atoms.

[0049] In formula (1), C 3 ~C 6 are each independently a single bond, —O—, —S—, —S—S—, —CO—, —CS—, —OCO—, —CH—, —OCH—, —CH═N—N═CH—, —NHCO—, —O—(C═O)—O—, —CH 2 —(C═O)—O—, and —CH 2 represents a group selected from the group consisting of O—(C═O)—;

[0050] In formula (1), M represents a mesogenic group. Specifically, M represents a group in which two to four identical or different skeletons selected from the group consisting of azomethines, azoxys, phenyls, biphenyls, terphenyls, naphthalenes, anthracenes, benzoates, cyclohexanecarboxylic acid phenyl esters, cyanophenylcyclohexanes, cyano-substituted phenylpyrimidines, alkoxy-substituted phenylpyrimidines, phenyldioxanes, tolanes, and alkenylcyclohexylbenzonitriles, which may be unsubstituted or have a substituent, are bonded together by a bonding group such as —O—, —S—, —S—S—, —CO—, —CS—, —OCO—, —CH—, —OCH—, —CH═N—N═CH—, —NHCO—, —O—(C═O)—O—, —CH—(C═O)—O—, or —CHO—(C═O)—.

[0051] Examples of the substituent that the mesogenic group M may have include a halogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, a cyano group, a nitro group, and —O—R 5 , -OC(=O)-R 5 , -C(=O)-OR 5 , -OC(=O)-OR 5 , -NR 5 -C(=O)-R 5 , -C(=O)-NR5 R 7 or —O—C(═O)—NR 5 R 7 Here, R 5 and R 7 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. 5 and R 7 is an alkyl group, the alkyl group may include —O—, —S—, —O—C(═O)—, —C(═O)—O—, —O—C(═O)—O—, —NR 6 -C(=O)-, -C(=O)-NR 6 -, -NR 6 - or -C(=O)- may be present (excluding the case where two or more adjacent -O- and -S- are present). 6 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

[0052] Examples of the substituent in the "alkyl group having 1 to 10 carbon atoms which may have a substituent" include a halogen atom, a hydroxyl group, a carboxyl group, a cyano group, an amino group, an alkoxy group having 1 to 6 carbon atoms, an alkoxyalkoxy group having 2 to 8 carbon atoms, an alkoxyalkoxyalkoxy group having 3 to 15 carbon atoms, an alkoxycarbonyl group having 2 to 7 carbon atoms, an alkylcarbonyloxy group having 2 to 7 carbon atoms, and an alkoxycarbonyloxy group having 2 to 7 carbon atoms.

[0053] The rod-shaped liquid crystal compound preferably has an asymmetric structure. Here, the asymmetric structure is a structure in which, in formula (1), R 3 -C 3 -D 3 -C 5 -M- and -M-C 6 -D 4 -C 4 -R 4 The term "asymmetric" refers to a structure that differs from the "asymmetric" structure. By using a rod-like liquid crystal compound with an asymmetric structure, the alignment uniformity can be further improved.

[0054] Preferred specific examples of the rod-shaped liquid crystal compound include the following compounds (B1) to (B12), although the rod-shaped liquid crystal compound is not limited to the following compounds.

[0055]

[0056]

[0057]

[0058] When the liquid crystal composition contains the rod-shaped liquid crystal compound, the liquid crystal composition preferably contains a compound represented by formula (2) as an alignment aid in combination with the rod-shaped liquid crystal compound. 1 -A 1 -B-A 2 -R 2 (2)

[0059] In formula (2), R 1 and R 2 are each independently a group selected from the group consisting of a linear or branched alkyl group having 1 to 20 carbon atoms, a linear or branched alkylene oxide group having 1 to 20 carbon atoms, a hydrogen atom, a halogen atom, a hydroxyl group, a carboxyl group, a (meth)acrylic group which may have an optional bonding group interposed therebetween, an epoxy group, a mercapto group, an isocyanate group, an amino group, and a cyano group.

[0060] The alkyl group and alkylene oxide group may be unsubstituted or substituted with one or more halogen atoms. Furthermore, the halogen atom, hydroxyl group, carboxyl group, (meth)acrylic group, epoxy group, mercapto group, isocyanate group, amino group, and cyano group may be bonded to the alkyl group having 1 to 2 carbon atoms and the alkylene oxide group.

[0061] R 1 and R 2 Preferred examples of the alkyl group include a halogen atom, a hydroxyl group, a carboxyl group, a (meth)acrylic group, an epoxy group, a mercapto group, an isocyanate group, an amino group, and a cyano group.

[0062] Also, R1 and R 2 At least one of R is preferably a reactive group. 1 and R 2 By having a reactive group as at least one of the above, the compound represented by formula (2) is fixed in the cured layer of the liquid crystal composition upon curing, and a stronger layer can be formed. Here, examples of the reactive group include a carboxyl group, a (meth)acrylic group, an epoxy group, a mercapto group, an isocyanate group, and an amino group.

[0063] In formula (2), A 1 and A 2 each independently represents a group selected from the group consisting of a 1,4-phenylene group, a 1,4-cyclohexylene group, a cyclohexen-1,4-ylene group, a 4,4'-biphenylene group, a 4,4'-bicyclohexylene group, and a 2,6-naphthylene group. The 1,4-phenylene group, the 1,4-cyclohexylene group, the cyclohexen-1,4-ylene group, the 4,4'-biphenylene group, the 4,4'-bicyclohexylene group, and the 2,6-naphthylene group may be unsubstituted or may be substituted with one or more substituents such as a halogen atom, a hydroxyl group, a carboxyl group, a cyano group, an amino group, an alkyl group having 1 to 10 carbon atoms, or a halogenated alkyl group. A 1 and A 2 In each of the groups, when two or more substituents are present, they may be the same or different.

[0064] A 1 and A 2 Particularly preferred examples of the aromatic ring skeleton include a group selected from the group consisting of a 1,4-phenylene group, a 4,4'-biphenylene group, and a 2,6-naphthylene group. These aromatic ring skeletons are relatively rigid compared to alicyclic skeletons, have high affinity with the mesogens of rod-like liquid crystal compounds, and result in higher alignment uniformity.

[0065] In formula (2), B is a single bond, —O—, —S—, —S—S—, —CO—, —CS—, —OCO—, or —CH 2 -, -OCH 2-, -CH=N-N=CH-, -NHCO-, -O-(C=O)-O-, -CH2-(C=O)-O-, and -CH 2 Particularly preferred examples of B include a single bond, —O—(C═O)—, and —CH═N—N═CH—.

[0066] Particularly preferred specific examples of the compound represented by formula (2) include the following compounds (A1) to (A10). These may be used alone or in combination of two or more in any ratio.

[0067]

[0068] In the above compound (A3), "*" represents a chiral center.

[0069] The weight ratio (total weight of compounds represented by Formula (2)) / (total weight of rod-shaped liquid crystal compounds) is preferably 0.001 or more, more preferably 0.01 or more, even more preferably 0.05 or more, and preferably 1 or less, more preferably 0.65 or less. By setting the weight ratio at or above the lower limit, the alignment uniformity in the liquid crystal composition layer can be improved. Furthermore, by setting the weight ratio at or below the upper limit, the alignment uniformity can be increased. Furthermore, the stability of the liquid crystal phase of the liquid crystal composition can be improved. Furthermore, since the refractive index anisotropy Δn of the liquid crystal composition can be increased, a cured layer of the liquid crystal composition having desired optical properties, such as selective reflection of circularly polarized light, can be stably obtained. Here, the total weight of the compounds represented by Formula (2) refers to the weight when only one type of compound represented by Formula (2) is used, and refers to the total weight when two or more types are used. Similarly, the total weight of the rod-shaped liquid crystal compounds refers to the weight when only one type of rod-shaped liquid crystal compound is used, and refers to the total weight when two or more types are used.

[0070] When the compound represented by formula (2) is used in combination with a rod-shaped liquid crystal compound, the molecular weight of the compound represented by formula (2) is preferably less than 600, and the molecular weight of the rod-shaped liquid crystal compound is preferably at least 600. This allows the compound represented by formula (2) to enter into gaps in the rod-shaped liquid crystal compound having a larger molecular weight, thereby improving the alignment uniformity.

[0071] The liquid crystal composition for forming the cured cholesteric liquid crystal layer may further contain optional components constituting the cured cholesteric liquid crystal layer and a solvent for facilitating handling of the liquid crystal composition. Examples of the optional components include a chiral agent, a polymerization initiator, and a surfactant. Specific examples of the optional components and solvents include those described in JP 2019-188740 A, as well as surfactants such as F-563 from DIC Corporation and KZ-GDP02 and KZ-GDP05 from AGC Seimi Chemical Co., Ltd., with F-563 from DIC Corporation and KZ-GDP02 and KZ-GDP05 from AGC Seimi Chemical Co., Ltd. being preferred as surfactants having a fluoroalkyl group chain length of less than 6.

[0072] A liquid crystal composition is applied to the surface of a support having an alignment control force to form a layer of the liquid crystal composition, which is then aligned to a cholesteric liquid crystal phase and cured to obtain a cholesteric liquid crystal cured layer. Examples of the support having an alignment control force include a film whose surface has been subjected to a rubbing treatment and a film whose surface has been given an alignment control force by stretching.

[0073] Although the liquid crystal composition may be aligned into a cholesteric liquid crystal phase immediately after application, alignment can be achieved by, if necessary, applying a treatment such as heating to create conditions conducive to the cholesteric liquid crystal phase. The curing method for curing the liquid crystal composition can be selected according to the components contained in the cholesteric liquid crystal composition. A layer of the cholesteric liquid crystal composition is typically cured by polymerizing a polymerizable component, such as a polymerizable liquid crystal compound, contained in the cholesteric liquid crystal composition. Examples of polymerization methods include a method of irradiating active energy rays and a thermal polymerization method. Among these, a method of irradiating active energy rays is preferred because it allows the polymerization reaction to proceed at room temperature. The active energy rays irradiated here may include any energy ray, such as visible light, ultraviolet light, and infrared light, as well as electron beams. When a layer of the cholesteric liquid crystal composition is cured by irradiating active energy rays, the preferred intensity of the irradiated active energy rays varies depending on the liquid crystal composition used, but is, for example, 50 mJ / cm. 2 ~10,000mJ / cm 2 It is possible.

[0074] Furthermore, after aligning the liquid crystal compound, the layer of the cholesteric liquid crystal composition may be subjected to a broadening treatment before curing the layer of the cholesteric liquid crystal composition. Such a broadening treatment can be carried out, for example, by combining one or more irradiation treatments with active energy rays and heating treatments. In this case, the energy of the irradiated light varies depending on the liquid crystal composition used, but is, for example, 0.01 mJ / cm. 2 ~50 mJ / cm 2 The heat treatment can be carried out, for example, by heating to a temperature of preferably 40° C. or higher, more preferably 50° C. or higher, and preferably 200° C. or lower, more preferably 140° C. or lower. By carrying out such a band-broadening treatment, the pitch of the helical structure can be continuously and greatly changed, thereby obtaining a wide reflection wavelength band.

[0075] The reflectance of the cured cholesteric liquid crystal layer to unpolarized light incident on the cured cholesteric liquid crystal layer is up to 50%. The cured cholesteric liquid crystal layer visually exhibits various colors depending on the reflection band and reflectance. When the reflectance of the cured cholesteric liquid crystal layer to unpolarized light incident on the cured cholesteric liquid crystal layer is 35 to 50% for all wavelengths in the wavelength range of 420 nm to 650 nm, the cured cholesteric liquid crystal layer is observed as a silvery layer. In one embodiment, the cured cholesteric liquid crystal layer preferably has a wide reflection wavelength band, and more preferably the reflection wavelength band includes a wavelength range of 420 nm to 650 nm. The "reflection wavelength band" refers to a wavelength range in which the reflectance of the cured cholesteric liquid crystal layer to unpolarized light incident on the cured cholesteric liquid crystal layer is 30% to 50%.

[0076] When the reflection wavelength band (the band in which 30 to 50% reflection occurs) is narrower than this, the cholesteric liquid crystal cured layer can exhibit various colors depending on the band. For example, when the center wavelength of the reflection band is around 450 nm, around 550 nm, or around 650 nm, the layer can exhibit colors such as blue, green, and red, respectively. The center wavelength of the reflection band can be adjusted by the type and proportion of the materials constituting the cured liquid crystal layer, as well as the manufacturing conditions of the cured liquid crystal layer. In particular, when manufacturing a cured liquid crystal layer having cholesteric regularity, the helical pitch of the cholesteric regularity can be adjusted by the type and proportion of the liquid crystal compound and chiral agent, and the chiral agent content. In particular, slight pitch adjustment can be easily achieved by changing the chiral agent content. Such adjustments make it possible to easily adjust the center wavelength of the reflection band to a desired value.

[0077] A plurality of cholesteric liquid crystal cured layers having different center wavelengths in the reflection band may be laminated. For example, a plurality of cholesteric liquid crystal cured layers may be laminated to form a cholesteric liquid crystal cured layer having a wide reflection band as a whole. An appropriate adhesive may be used for lamination, if necessary.

[0078] (Retardation Layer) The small fragment layer may include an optional layer in addition to the cholesteric liquid crystal cured layer. An example of the optional layer is a retardation layer. The retardation layer is a layer that imparts a retardation to incident light, preferably a layer that imparts an in-plane retardation to incident light. Hereinafter, a small fragment layer including a retardation layer in addition to the cholesteric liquid crystal cured layer is referred to as an optical layer. Some of the multiple small fragment layers included in the dividing layer may be optical layers, or all of the multiple small fragment layers may be optical layers. The retardation layer included in the optical layer may have a single-layer structure or a multi-layer structure. For example, the retardation layer included in the optical layer may be a laminate of two or more layers having different in-plane retardation values, for example, the retardation layer may be a laminate of a layer that functions as a λ / 4 plate and a layer that functions as a λ / 2 plate.

[0079] The in-plane retardation value of the retardation layer is not particularly limited. In one embodiment, the dividing layer preferably includes an optical layer including a retardation layer that is a λ / 4 plate. When non-polarized light is incident on the transferred object, the optical layer including a retardation layer that is a λ / 4 plate imparts a phase difference of λ / 4 or close to λ / 4 to the circularly polarized light reflected by the cholesteric liquid crystal cured layer and emits it as linearly polarized light. Therefore, the transferred object can exhibit high discrimination function when observed using a viewer including a linear polarizer (for example, polarized sunglasses including a linear polarizer).

[0080] Here, unless otherwise specified, the λ / 4 plate means a layer having an in-plane retardation value of (λ / 4-30 nm) or more (λ / 4+30 nm) at a measurement wavelength λ. The in-plane retardation value of the retardation layer that is a λ / 4 plate that can be included in the dividing layer is usually (λ / 4-30 nm) or more, preferably (λ / 4-15 nm) or more, more preferably (λ / 4-10 nm) or more, and is usually (λ / 4+30 nm) or less, preferably (λ / 4+15 nm) or less, more preferably (λ / 4+10 nm) or less, and ideally λ / 4.

[0081] In another embodiment, the dividing layer preferably includes an optical layer including a retardation layer that is a λ / 2 plate. When unpolarized light is incident on the transferred object, the optical layer including a retardation layer that is a λ / 2 plate imparts a phase difference of λ / 2 or close to λ / 2 to circularly polarized light having a predetermined rotation direction reflected by the cholesteric liquid crystal cured layer, and emits the light as circularly polarized light having a rotation direction opposite to the predetermined rotation direction. Therefore, the transferred object can exhibit high discrimination function when observed using a viewer including a circular polarizer.

[0082] Here, unless otherwise specified, the term "lambda / 2 plate" refers to a layer having an in-plane retardation value at a measurement wavelength λ of (lambda / 2 - 60 nm) or more (lambda / 2 + 60 nm). The in-plane retardation value of the retardation layer, which is a lambda / 2 plate that can be included in the dividing layer, is usually (lambda / 2 - 60 nm) or more, preferably (lambda / 2 - 50 nm) or more, more preferably (lambda / 2 - 40 nm) or more, even more preferably (lambda / 2 - 30 nm) or more, even more preferably (lambda / 2 - 20 nm) or more, and is usually (lambda / 2 + 60 nm) or less, preferably (lambda / 2 + 50 nm) or less, more preferably (lambda / 2 + 40 nm) or less, even more preferably (lambda / 2 + 30 nm) or less, even more preferably (lambda / 2 + 20 nm) or less, and ideally lambda / 2.

[0083] The dividing layer may contain two or more types of optical layers as small fragment layers. Examples of two or more types of optical layers include optical layers in which the in-plane retardation values ​​of the included retardation layers are different from each other. In one embodiment, the dividing layer contains two types of optical layers as small fragment layers, and the absolute value of the difference between the in-plane retardation values ​​of the two types of optical layers is preferably λ / 2 or a value close to λ / 2 at the measurement wavelength λ, specifically, preferably (λ / 2-60nm) or more, more preferably (λ / 2-50nm) or more, even more preferably (λ / 2-40nm) or more, even more preferably (λ / 2-30nm) or more, preferably (λ / 2+60nm) or less, more preferably (λ / 2+50nm) or less, even more preferably (λ / 2+40nm) or less, even more preferably (λ / 2+30nm) or less, and ideally λ / 2.

[0084] When the dividing layer includes two optical layers as small fragment layers, when unpolarized light is incident on the transfer, the long axis (if the polarized light is elliptically polarized) or transmission axis (if the polarized light is linearly polarized) of the polarized light emitted to the viewing side from the optical layer with a relatively small in-plane retardation value of the two optical layers becomes orthogonal or nearly orthogonal to the long axis (if the polarized light is elliptically polarized) or transmission axis (if the polarized light is linearly polarized) of the polarized light emitted to the viewing side from the optical layer with a relatively large in-plane retardation value. Therefore, when unpolarized light is incident on the transfer and observed with a viewer including a linear polarizer, the amount of light reflected by one optical layer is theoretically zero, and the amount of light reflected by the other optical layer is theoretically the same as the amount of light reflected by the cholesteric liquid crystal cured layer, which is half the amount of unpolarized light incident on the transfer, resulting in extremely high contrast between the two optical layers. Therefore, the transfer can exhibit high discrimination capabilities.

[0085] In this embodiment, the dividing layer may include an optional small piece layer in addition to the two optical layers having an absolute value of in-plane retardation within the above range.Examples of the optional small piece layer include a small piece layer including an isotropic layer having an in-plane retardation value of 0 nm or close to 0 nm in addition to a cholesteric liquid crystal hardened layer.The in-plane retardation value of the isotropic layer that can be included in the small piece layer is preferably 30 nm or less, more preferably 20 nm or less, even more preferably 10 nm or less, usually 0 nm or more, and may be 0 nm.

[0086] The optical layer including the retardation layer is preferably arranged on the adhesive layer in a pattern. When the optical layer is arranged in a pattern, the transferred product can display a pattern when the transferred product of the transfer laminate sheet is observed with a viewer equipped with a linear polarizer or the like, so that the transferred product can exhibit high identification function and have excellent design properties.

[0087] When the optical layer is disposed on the adhesive layer in a pattern, the pattern may have any shape, such as letters, numbers, symbols, pictures, etc.

[0088] 1.5. First Embodiment of Transfer Laminate Sheet A first embodiment of the transfer laminate sheet will be described below with reference to the drawings. FIG. 1 is a cross-sectional view schematically illustrating a transfer laminate sheet according to the first embodiment of the present invention. As shown in FIG. 1, the transfer laminate sheet 100 according to the first embodiment includes a release base layer 110, an adhesive layer 120, and a dividing layer 130, in this order when viewed from the thickness direction. A main surface 120D of the adhesive layer 120 is directly connected to the release base layer 110. The dividing layer 130 is directly connected to a main surface 120U of the adhesive layer 120. The dividing layer 130 includes a plurality of small fragment layers each formed as a cured cholesteric liquid crystal layer 141. The plurality of small fragment layers (cured cholesteric liquid crystal layer) 141 are divided by cracks 150.

[0089] 1.6. Second Embodiment of Transfer Laminate Sheet A second embodiment of the transfer laminate sheet will be described below with reference to the drawings. The dividing layer of the transfer laminate sheet according to the second embodiment includes an optical layer including a cured cholesteric liquid crystal layer and a retardation layer as a small layer. FIG. 2 is a cross-sectional view schematically illustrating a transfer laminate sheet according to the second embodiment of the present invention. As shown in FIG. 2, the transfer laminate sheet 200 according to the second embodiment includes a release substrate layer 110, an adhesive layer 120, and a dividing layer 230, in this order when viewed from the thickness direction. The dividing layer 230 includes an optical layer 240 as a plurality of small layers divided by cracks 250. The optical layer 240 includes a cured cholesteric liquid crystal layer 241 and a retardation layer 242. The retardation layer 242 is disposed between the cured cholesteric liquid crystal layer 241 and the adhesive layer 120. The dividing layer 230 is directly attached to the main surface 120U of the adhesive layer 120. In detail, the retardation layer 242 included in the optical layer 240 is directly on the main surface 120U of the adhesive layer 120. The optical layer 240 as a plurality of small fragment layers is divided by cracks 250. The in-plane retardation value of the retardation layer 242 is arbitrary, but may be a λ / 2 plate or a λ / 4 plate. In this embodiment, all of the plurality of small fragment layers included in the dividing layer 230 are optical layers 240, but in another embodiment, only some of the plurality of small fragment layers may be optical layers 240 including the retardation layer 242, and the dividing layer 230 may include, in addition to the optical layer 240, a small fragment layer including, for example, a cholesteric liquid crystal cured layer and an isotropic layer.

[0090] 1.7. Transfer Laminate Sheet Embodiment 3 A transfer laminate sheet embodiment 3 will be described below with reference to the drawings. The dividing layer of the transfer laminate sheet according to embodiment 3 includes two or more optical layers as small fragment layers. FIG. 3 is a cross-sectional view schematically illustrating a transfer laminate sheet according to embodiment 3 of the present invention. As shown in FIG. 3, the transfer laminate sheet 300 according to embodiment 3 includes a release substrate layer 110, an adhesive layer 120, and a dividing layer 330, in this order when viewed from the thickness direction. The dividing layer 330 includes optical layers 340a and 340b as a plurality of small fragment layers divided by cracks 350. The optical layer 340a includes a retardation layer 342, a retardation layer 343, and a cured cholesteric liquid crystal layer 341. The retardation layer 342 and the retardation layer 343 are disposed between the cured cholesteric liquid crystal layer 341 and the adhesive layer 120. The retardation layer 343 is in direct contact with the main surface 120U of the adhesive layer 120. The retardation layer 342 is a λ / 4 plate, and the retardation layer 343 is a λ / 2 plate. The optical layer 340b includes the retardation layer 342, an isotropic layer 344, and a cured cholesteric liquid crystal layer 341. The retardation layer 342 and the isotropic layer 344 are disposed between the cured cholesteric liquid crystal layer 341 and the adhesive layer 120. The in-plane retardation value of the isotropic layer 344 is 0 nm. The isotropic layer 344 is in direct contact with the main surface 120U of the adhesive layer 120. In this embodiment, the absolute value of the difference between the in-plane retardation value of the optical layer 340a and the in-plane retardation value of the optical layer 340b corresponds to the absolute value of the difference between the in-plane retardation value of the retardation layer 343 and the in-plane retardation value of the isotropic layer 344, and in this embodiment, it is λ / 2 or close to λ / 2, for example, within the range of (λ / 2±60 nm). In this embodiment, all of the multiple small fragment layers included in the dividing layer 330 are optical layers 340a or optical layers 340b, but in another embodiment, only some of the multiple small fragment layers may be optical layers 340a or optical layers 340b, and the dividing layer 330 may include, in addition to the optical layers 340a and 340b, a small fragment layer including, for example, a cholesteric liquid crystal cured layer and an isotropic layer.

[0091] <2. Manufacturing method of transfer laminate sheet> The transfer laminate sheet can be manufactured by any manufacturing method. From the viewpoint of effectively obtaining the advantage of the present invention that the transfer laminate sheet can be easily manufactured, it is preferable to manufacture the transfer laminate sheet by the manufacturing method described below.

[0092] A preferred method for producing a transfer laminate sheet includes the steps of: (1) preparing a first laminate including, in this order, the release substrate layer, the adhesive layer, and a layer (A) directly on the adhesive layer and including the cholesteric liquid crystal cured layer; and (2) forming cracks in the layer (A) included in the first laminate to divide the layer (A) and form a plurality of small fragment layers. Hereinafter, a method for producing a transfer laminate sheet according to a preferred embodiment of the present invention will be described.

[0093] <2.1. Step (1)> In step (1), a first laminate is prepared. The first laminate includes a release substrate, an adhesive layer, and a layer (A) including a cured cholesteric liquid crystal layer, in this order when viewed from the thickness direction. The layer (A) has a layer structure corresponding to the dividing layer included in the transfer laminate sheet. For example, when the dividing layer includes a retardation layer in addition to the cured cholesteric liquid crystal layer, a first laminate including a layer (A) including the cured cholesteric liquid crystal layer and the retardation layer is prepared. Also, for example, when some of the multiple small fragment layers included in the dividing layer are optical layers and the optical layer is arranged on the adhesive layer in a pattern, a first laminate including a layer (A) having a pattern corresponding to the pattern of the optical layer is prepared. The first laminate is preferably long from the viewpoint of efficiently manufacturing the transfer laminate sheet.

[0094] The first laminate can be manufactured by any manufacturing method. The first laminate may be manufactured by laminating the layer (A) and a release substrate via an adhesive layer. Alternatively, a laminate may be obtained by laminating a portion of the layer (A) and a release substrate via an adhesive layer, and then laminating the remaining layers of the layer (A) onto the resulting laminate to obtain the first laminate. For example, when the layer (A) is a cured cholesteric liquid crystal layer, the cured cholesteric liquid crystal layer may be formed on the surface of a support having an alignment regulating force, and the resulting cured cholesteric liquid crystal layer may be attached to a release substrate via an adhesive layer. Furthermore, when the layer (A) includes a cured cholesteric liquid crystal layer and a retardation layer, the retardation layer may be laminated on the cured cholesteric liquid crystal layer to obtain a laminate, and the resulting laminate may be laminated on a release substrate via an adhesive layer to obtain the first laminate. The layer (A) having a pattern corresponding to the pattern of the optical layer may be obtained, for example, by laminating a cured cholesteric liquid crystal layer and a patterned retardation layer. The patterned retardation layer may be obtained, for example, by forming a layer of a liquid crystal composition on the surface of a support, homogeneously aligning a polymerizable liquid crystal compound contained in the liquid crystal composition, and curing the liquid crystal composition in a pattern using a mask or the like while maintaining the alignment. Here, homogeneously aligning a polymerizable liquid crystal compound means forming a layer containing the liquid crystal compound and aligning the direction of the maximum refractive index in the refractive index ellipsoid of the molecules of the liquid crystal compound in the layer in a certain direction parallel to the surface of the layer.

[0095] <2.2. Step (2)> In step (2), cracks are formed in the layer (A) included in the first laminate to divide the layer (A) and form a plurality of small layer fragments. Any method for forming the cracks is possible. From the viewpoint of effectively obtaining the advantages of the present invention, the cracks can be formed by pressing a processing tool having an uneven shape against the layer (A) side of the first laminate. Preferably, the cracks are formed by pressing the first laminate between the support tool and the processing tool while the first laminate is supported by the support tool.

[0096] As the processing tool, a member having convex portions on its surface corresponding to the shape of the crack as viewed from the thickness direction of the layer (A) can be used. For example, if the shape of the crack as viewed from the thickness direction of the layer (A) is lattice-shaped, a member having lattice-shaped convex portions on its surface can be used. Only one processing tool may be used, or two or more processing tools may be used in combination. For example, a processing tool having convex portions on its surface corresponding to one part of the crack and a processing tool having convex portions on its surface corresponding to another part of the crack may be used in combination.

[0097] The same processing tool may be pressed against the layer (A) multiple times in different positions to form cracks, or a cylindrical processing tool may be used to form continuous cracks in the layer (A).

[0098] As a method for forming cracks in step (2), for example, the method described in International Publication No. 2021 / 172567 (Patent Document 2) can be used.

[0099] When a transfer laminate sheet is obtained by pressing the convex portion of a processing tool against layer (A) included in a first laminate to divide layer (A) and form multiple small fragment layers, the following advantages are obtained. Because the first laminate has an adhesive layer between the release substrate and layer (A), when the processing tool is removed from the transfer laminate sheet on which multiple small fragment layers have been formed, the small fragment layers are less likely to adhere to the processing tool and peel off from the release substrate. Therefore, the resulting transfer laminate sheet has reduced chipping of the small fragment layers, and therefore reduced chipping of the divided layers. Because chipping of the divided layers is reduced, the transfer product obtained by transferring the transfer laminate sheet to a display substrate also has reduced chipping and improved clarity.

[0100] 3. Display Medium Manufacturing Method> A display medium with an identification function can be manufactured by transferring the transfer laminate sheet to a display substrate. The display medium includes a display substrate, a second adhesive layer, and a dividing layer, in this order, and the dividing layer includes a plurality of small fragment layers including a cured cholesteric liquid crystal layer and divided by cracks. The display medium manufacturing method preferably includes the following steps: manufacturing the transfer laminate sheet by a process including step (1) and then step (2); forming a patterned second adhesive layer on a portion of the dividing layer of the transfer laminate sheet to obtain a transfer laminate seal; attaching the second adhesive layer side of the transfer laminate seal to a display substrate; and peeling off the release substrate and the adhesive layer of the transfer laminate seal to obtain a display medium (5).

[0101] In step (3), the method for forming the patterned second adhesive layer is arbitrary. Examples of the method for forming the second adhesive layer include a method of applying an adhesive directly onto the dividing layer in a patterned form; and a method of transferring a separately formed patterned adhesive layer onto the dividing layer. Examples of methods for applying the adhesive include screen printing, inkjet printing, and gravure printing. Screen printing is preferred because it can easily form a fine pattern.

[0102] In step (3), the peel strength P3 between the patterned second adhesive layer and the dividing layer is preferably 4 N / 25 mm or more, more preferably 5 N / 25 mm or more, and even more preferably 6 N / 25 mm or more. The upper limit is not particularly limited, but can be, for example, 10 N / 25 mm or less. When the peel strength P3 is equal to or greater than the lower limit, the dividing layer is less likely to separate from the adherend, and the durability of the transferred product is improved.

[0103] The difference (P3-P1) between the peel strength P3 between the second adhesive layer and the dividing layer and the peel strength P1 between the adhesive layer and the dividing layer included in the transfer laminate sheet is preferably 1.2 N / 25 mm or more, more preferably 2.0 N / 25 mm or more, and even more preferably 3.5 N / 25 mm or more. The upper limit is not particularly limited, but can be, for example, 5 N / 25 mm or less. If the difference (P3-P1) is equal to or greater than the lower limit, when the release substrate and adhesive layer included in the transfer laminate seal are peeled off in step (5), the dividing layer is less likely to peel off together with the release substrate and adhesive layer.

[0104] In step (4), the display substrate to which the transfer laminated seal is attached may be made of any material. For example, organic materials, inorganic materials, and composite materials combining these materials may be used as the display substrate material. Specific examples of the display substrate material include resin, paper, cloth, leather, metal, alloy, and glass.

[0105] <4. Uses of Transfer Laminate Sheet and Display Medium> The transfer laminate sheet described above has reduced chipping of the transferred material, and can therefore be suitably used, for example, to form a display medium. At least a portion of the multiple fragment layers, including the cholesteric liquid crystal cured layer, contained in the transfer laminate sheet is transferred onto a display substrate to form a display medium. The fragment layers contained in the display medium include a cholesteric liquid crystal cured layer having a circularly polarized light separation function, so that when the display medium is irradiated with unpolarized light and observed with the naked eye, reflected light can be seen. On the other hand, when the display medium is irradiated with polarized light, or when unpolarized light is irradiated and the reflected light is observed with a viewer that can selectively transmit polarized light, such as a circular polarizer or a linear polarizer, the display due to the reflected light from the fragment layers contained in the display medium differs from when irradiated with unpolarized light and observed with the naked eye, depending on the optical properties of the fragment layers, such as the direction of polarization rotation that can be reflected by the cholesteric liquid crystal cured layer contained in the fragment layer and the in-plane retardation value of the retardation layer that can be contained in the fragment layer. For example, when the small piece layer is a cholesteric liquid crystal cured layer and the small piece layer is observed under non-polarized light through a circular polarizer that does not transmit reflective circularly polarized light, the reflected light of the small piece layer may be difficult to see. Also, for example, when the small piece layer is an optical layer including a cholesteric liquid crystal cured layer and a λ / 4 plate as a retardation layer and observed under non-polarized light through a linear polarizer, the reflected light of the small piece layer changes in brightness depending on the relationship between the in-plane slow axis of the small piece layer and the transmission axis of the linear polarizer. Also, for example, by forming a pattern using a plurality of small piece layer groups with different in-plane retardation values, it is possible to obtain a display medium that cannot be seen by naked eye observation under non-polarized light, but when observed using a viewer that can selectively transmit polarized light, it is possible to obtain a display medium that can display a pattern different from that observed by naked eye depending on the in-plane retardation value of the small piece layer group.

[0106] Display media obtained from the transfer laminate sheet have reduced chipping and can provide images that differ from those observed with the naked eye. Therefore, the transfer laminate sheet is useful for producing display media that are highly difficult to counterfeit.

[0107] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the examples shown below, and can be practiced with any modifications within the scope of the claims of the present invention and their equivalents.

[0108] In the following description, the "%" and "parts" that represent amounts are by weight unless otherwise specified. Furthermore, the operations described below were carried out at room temperature (20°C ± 15°C) and atmospheric pressure (1 atm) unless otherwise specified.

[0109] <Evaluation Method> (Detachment of Cured Liquid Crystal Layer) In each example, the surface of the cured liquid crystal layer after cracking was visually observed, and the number of detached portions of the cured liquid crystal layer was counted. The fewer detached portions of the cured liquid crystal layer, the clearer the outline of the pattern shape and the less chipping there is inside the pattern, making it possible to obtain a transferred product. The detachment of the cured liquid crystal layer was evaluated according to the following criteria: "Excellent": Less than 5 detached portions of the cured liquid crystal layer "Good": 5 to less than 10 detached portions of the cured liquid crystal layer "Poor": 10 or more detached portions of the cured liquid crystal layer

[0110] (Clarity of Transfer) In each example, chipping was visually observed at the outline of the pattern shape of the transfer and inside the pattern, and the clarity of the transfer was evaluated according to the following criteria: "Excellent": No chipping was found at either the outline of the pattern shape of the transfer or inside the pattern. "Good": Chips were found at either the outline of the pattern shape of the transfer or inside the pattern, but no chipping was found at the other. "Poor": Chips were found at both the outline of the pattern shape of the transfer and inside the pattern.

[0111] (Method for Measuring Peel Strength) The peel strength between the cured liquid crystal layer and the adhesive layer was measured using a "Digital Force Gauge ZP50" manufactured by IMADA Co., Ltd., in accordance with JIS Z0237, at a temperature of 23°C, a peel speed of 300 m / min, and peeling in a 180° direction. A rectangular test piece measuring 25 mm x 150 mm was cut from the laminate to be measured and used as the measurement sample.

[0112] (Method for Measuring In-Plane Retardation) The in-plane retardation was measured at a measurement wavelength of 550 nm using a retardation meter (Axoscan manufactured by Axometrics).

[0113] (Method for measuring reflectance of cured cholesteric liquid crystal layer) The support substrate film was peeled off from the multilayer film to obtain a cured cholesteric liquid crystal layer. The reflectance of this cured cholesteric liquid crystal layer when unpolarized light (wavelength 400 nm to 800 nm) was incident on the cured cholesteric liquid crystal layer was measured using an ultraviolet-visible spectrophotometer ("UV-Vis 550" manufactured by JASCO Corporation).

[0114] <Production Example 1: Production of broadband reflective cholesteric liquid crystal cured layer (CLC_W) capable of reflecting right-handed circularly polarized light> A liquid crystal composition was prepared by mixing 100 parts of a photopolymerizable liquid crystal compound represented by the following formula (X1) (the compound represented by the above formula (B5)), 25 parts of a photopolymerizable non-liquid crystal compound represented by the following formula (X2) (the compound represented by the above formula (A10)), 7.5 parts of a chiral agent ("LC756" manufactured by BASF), 5 parts of a photopolymerization initiator ("Irgacure 907" manufactured by Ciba Japan), 0.2 parts of a surfactant ("S-420" manufactured by AGC Seimi Chemical Co., Ltd.), and 120 parts of cyclopentanone and 200 parts of 1,3-dioxolane as solvents.

[0115]

[0116]

[0117] A long polyethylene terephthalate film ("A4300" manufactured by Toyobo Co., Ltd.; thickness: 100 μm) was prepared as a supporting substrate film. This supporting substrate film was attached to the feeding section of a film transport device, and the following operations were performed while transporting the supporting substrate film in the longitudinal direction.

[0118] The surface of the support substrate film was subjected to a rubbing treatment in the longitudinal direction parallel to the transport direction. Next, a liquid crystal composition was applied to the rubbed surface of the support substrate film using a die coater to form a liquid crystal composition layer. This liquid crystal composition layer was subjected to an alignment treatment by heating at 120°C for 5 minutes. Thereafter, the liquid crystal composition layer was subjected to a band broadening treatment. In this band broadening treatment, 5 to 30 mJ / cm2 The desired bandwidth was controlled by repeatedly alternating between weak ultraviolet irradiation at 900 mJ / cm and heating at 100 to 120°C. 2 The layer of liquid crystal composition was irradiated with ultraviolet light of 1000 kJ / cm 2 to cure the layer of liquid crystal composition. This resulted in a multilayer film comprising a supporting substrate film and a cured cholesteric liquid crystal layer. The reflectance of the cured cholesteric liquid crystal layer of this multilayer film was measured using the measurement method described above. As a result of the measurement, the cured cholesteric liquid crystal layer had a wavelength range from 450 nm to 700 nm in which the reflectance for unpolarized light was 40% or more, and the half-width of the selective reflection band was 250 nm. The film thickness of the cured cholesteric liquid crystal layer was adjusted to 5.3 μm.

[0119] <Production Example 2: Production of a red-reflecting cholesteric liquid crystal cured layer (CLC_R) capable of reflecting right-handed circularly polarized light> In Production Example 1, the chiral agent ("LC756" manufactured by BASF) was changed to 6.8 parts, and the wavelength was increased to 900 mJ / cm without performing the broadening treatment. 2 The layer of liquid crystal composition was irradiated with ultraviolet light of 1000 kJ / cm 2 to cure the layer of liquid crystal composition. Except for this, a multilayer film was produced in the same manner as in Production Example 1. The reflectance of the cured cholesteric liquid crystal layer of this multilayer film was measured using the same measurement method as in Production Example 1. As a result of the measurement, the cured cholesteric liquid crystal layer had a center wavelength near 650 nm, a half-width of about 20 nm, and a wavelength range that was visually recognized as red, with a reflectance of 40% or more for unpolarized light. The film thickness of the cured cholesteric liquid crystal layer was adjusted to 3.6 μm.

[0120] <Production Example 3: Production of a green-reflecting cholesteric liquid crystal layer (CLC_G) capable of reflecting right-handed circularly polarized light> In Production Example 1, the band-widening treatment was not performed and the green-reflecting cholesteric liquid crystal layer (CLC_G) was 900 mJ / cm 2The layer of liquid crystal composition was irradiated with ultraviolet light of 1000 kJ / cm 2 to harden the layer of liquid crystal composition. Except for this, a multilayer film was produced in the same manner as in Production Example 1. The reflectance of the cured cholesteric liquid crystal layer of this multilayer film was measured using the same measurement method as in Production Example 1. As a result of the measurement, the cured cholesteric liquid crystal layer had a center wavelength near 550 nm, a half-width of about 20 nm, and a wavelength range that was visually recognized as green, with a reflectance of 40% or more for unpolarized light. The film thickness of the cured cholesteric liquid crystal layer was adjusted to 3.6 μm.

[0121] <Production Example 4: Production of a blue-reflecting cholesteric liquid crystal cured layer (CLC_B) capable of reflecting right-handed circularly polarized light> In Production Example 1, the chiral agent (BASF "LC756") was changed to 9.5 parts, and the layer of liquid crystal composition was irradiated with 900 mJ / cm2 of ultraviolet light without performing a broadband treatment, thereby curing the layer of liquid crystal composition. A multilayer film was produced in the same manner as in Production Example 1. The reflectance of the cholesteric liquid crystal cured layer of this multilayer film was measured using the same measurement method as in Production Example 1. As a result of the measurement, the cholesteric liquid crystal cured layer had a center wavelength near 450 nm, a wavelength range with a half-width of approximately 20 nm, and a wavelength range in which the reflectance to unpolarized light was 40% or more, and which was visually recognized as blue. The film thickness of the cholesteric liquid crystal cured layer was adjusted to 3.6 μm.

[0122] <Production Example 5: Production of a liquid crystal cured layer having a phase difference of λ / 4> A liquid crystal composition was prepared by mixing 100 parts of a liquid crystal compound (LC242 manufactured by BASF), 12 parts of a polyfunctional methacrylate (TMPT manufactured by Shin-Nakamura Chemical Co., Ltd.), 4 parts of a photopolymerization initiator (Irgacure 379 manufactured by Ciba Japan), 0.15 parts of a surfactant (Megafac F-562 manufactured by DIC Corporation), 198 parts of methyl ethyl ketone as a solvent, and 53 parts of 1,3-dioxolane.

[0123] A long polyethylene terephthalate film ("A4300" manufactured by Toyobo Co., Ltd.; thickness: 100 μm) was prepared as a supporting substrate film. This supporting substrate film was attached to the feeding section of a film transport device, and the following operations were performed while transporting the supporting substrate film in the longitudinal direction.

[0124] The surface of the support substrate film was subjected to a rubbing treatment in the longitudinal direction parallel to the conveying direction. Next, a liquid crystal composition was applied to the rubbed surface of the support substrate film using a die coater to form a liquid crystal composition layer. This liquid crystal composition layer was subjected to an alignment treatment by heating at 120°C for 4 minutes (alignment treatment step). Thereafter, a 900 mJ / cm 2 The layer of liquid crystal composition was irradiated with ultraviolet light to harden the layer of liquid crystal composition (ultraviolet curing treatment). This resulted in a multilayer film comprising a support substrate film and a liquid crystal cured layer (retardation film layer) as a retardation layer. After bonding an adhesive sheet ("CS9621T" manufactured by Nitto Denko Corporation) to this multilayer film, quartz glass was further bonded to the surface of the adhesive sheet opposite the liquid crystal cured layer, thereby obtaining a laminate having a layer structure of quartz glass / adhesive layer / liquid crystal cured layer as a retardation layer / support substrate film. The support substrate film was peeled from this laminate, and the in-plane retardation of the cured liquid crystal layer was measured using the measurement method described above to obtain the in-plane retardation value of the cured liquid crystal layer. As a result of the measurement, the in-plane retardation of the cured liquid crystal layer at a wavelength of 550 nm was 140 nm, and the direction of the slow axis relative to the support substrate film was parallel to the longitudinal direction of the film and approximately 0 °. The film thickness of the cured liquid crystal layer was adjusted to 1.2 μm.

[0125] <Production Example 6: Production of a liquid crystal cured layer having a λ / 4 pattern retardation> In Production Example 5, a mask substrate on which a pattern was printed with black light-shielding ink was used as a supporting substrate film, and in the ultraviolet curing treatment after the alignment treatment step, 7.2 mJ / cm 2 The same operation as in Production Example 5 was performed to obtain a multilayer film comprising a mask substrate and a cured liquid crystal layer, except that the layer of the liquid crystal composition was irradiated with 900 mJ / cm2 of ultraviolet light while heated at 90 ° C. The in-plane retardation of the cured liquid crystal layer was then measured using the multilayer film in the same manner as in Production Example 5. The in-plane retardation of the portion corresponding to the light-shielding ink portion of the mask substrate was approximately 0 nm, and the in-plane retardation of the portion corresponding to the non-light-shielding ink portion was 140 nm, and a λ / 4 patterned retardation layer having a portion with a retardation value of λ / 4 in a pattern was formed.

[0126] <Production Example 7: Production of cured liquid crystal layer having λ / 2 pattern retardation> The same operation as in Production Example 6 was performed except that the thickness of the cured liquid crystal layer was set to 2.4 μm, to form a λ / 2 pattern retardation layer having a portion where the in-plane retardation was approximately 0 nm and a patterned portion where the in-plane retardation was 270 nm.

[0127] Examples 1 to 4, Comparative Examples 1 and 2 In the following Examples 1 to 4 and Comparative Examples 1 and 2, transfer laminate sheets having no retardation layer were produced, and the transferred products were evaluated.

[0128] Example 1 (Production of Laminate (A)) The surface of the liquid crystal cured layer of the laminate film produced in Production Example 1 and the surface of the adhesive layer (1) of the adhesive film ("PET75-H109" manufactured by Nichiei Shinka Co., Ltd.: a film comprising an adhesive layer (1) (thickness 20 μm) containing an acrylic adhesive and a transparent polyethylene terephthalate (PET) layer (thickness 75 μm)) were bonded together to obtain a laminate having a layer structure of supporting substrate film / liquid crystal cured layer / adhesive layer (1) / transparent PET layer. Then, the supporting substrate film was peeled off to obtain a laminate (A) as a first laminate having a layer structure of liquid crystal cured layer / adhesive layer (1) / transparent PET layer. In the laminate (A), the liquid crystal cured layer corresponds to layer (A), and the transparent PET layer corresponds to the peelable substrate layer.

[0129] (Production of a member (roll) having a textured shape) A metal roll made of stainless steel with electroless nickel plating (NiP plating) on ​​its surface was prepared. The plated surface of the roll was cut with a diamond bite (apex angle 50°) to obtain rolls A and B having multiple protrusions. For roll A, the multiple protrusions were formed so that the protrusions extended in a direction that formed a 45° angle to the right with respect to a straight line on the roll circumferential surface parallel to the roll axis, with a pitch of 50 μm, and the angle of the apex of the protrusions was 50° in a cross section perpendicular to the direction in which the protrusions extended. For roll B, the multiple protrusions were formed so that the protrusions extended in a direction that formed a 45° angle to the left with respect to a straight line on the roll circumferential surface parallel to the roll axis, with a pitch of 50 μm, and the angle of the apex of the protrusions was 50° in a cross section perpendicular to the direction in which the protrusions extended.

[0130] (Crack Formation Step) Roll A was pressed against the laminate (A) from the side of the cured liquid crystal layer (press pressure 10 MPa), and then roll B was pressed against the laminate (A) (press pressure 10 MPa) to form cracks in the laminate (A). At this time, the side of the laminate (A) opposite the cured liquid crystal layer (transparent PET layer side, backup roll side) was supported by a backup roll. A roll with a surface hardness of D70 was used as the backup roll. Here, the hardness is a value measured using a durometer (type D) in accordance with JIS K-6253. The same applies hereinafter. As a result, the cured liquid crystal layer of the laminate (A) was divided into square pieces (major axis 70 μm) with sides of 50 μm when viewed from the thickness direction of the cured liquid crystal layer, to obtain a transfer laminate sheet (A).

[0131] The cross section of the transfer laminate sheet (A) that had undergone the crack formation process was observed with a scanning electron microscope to evaluate whether the cracks had reached a position deeper than the surface of the adhesive layer (1) of the transfer laminate sheet (A). The observation was performed on a cross section having a length of 500 μm in the plane direction at an arbitrary position on the transfer laminate sheet (A). As a result, it was found that cracks had formed on the entire surface of the transfer laminate sheet (A) to a position deeper than the surface of the adhesive layer (1).

[0132] The surface of the transfer laminate sheet (A) that had undergone the crack formation step was evaluated by the above-described method. The evaluation results are shown in Table 1.

[0133] (Transfer process) A pressure-sensitive adhesive (ThreeBond Co., Ltd. "1549", an acrylic adhesive) was printed in a pattern on the liquid crystal cured layer surface of the transfer laminate sheet (A) that had undergone the crack formation process using a screen printing plate to form a pressure-sensitive adhesive layer (2) as a second adhesive layer, and a transfer laminate sheet (A) with an adhesive layer (2) was obtained as a transfer laminate seal. The peel strength between the pressure-sensitive adhesive layer (2) and the liquid crystal cured layer was 4 N / 25 mm. After bonding the surface of the adhesive layer (2) of the transfer laminate sheet (A) with the adhesive layer (2) to the adherend (acrylic plate), the transparent PET layer and the adhesive layer (1) were peeled off, and the patterned liquid crystal cured layer was transferred to the adherend, obtaining a patterned transfer product.

[0134] (Evaluation of Transferred Product) The cured liquid crystal layer transferred to the adherend was evaluated by the above-mentioned method. The evaluation results are shown in Table 1.

[0135] Example 2 In Example 1, the cholesteric liquid crystal cured layer (CLC_G) produced in Production Example 3 was used as the liquid crystal cured layer, and the adhesive film was "RB105" manufactured by Nichiei Shinka Co., Ltd. (a film comprising an adhesive layer (1) (thickness 20 μm) containing an acrylic adhesive and a transparent PET layer (thickness 75 μm)). Except for the above, the same operations as in Example 1 were performed to form a laminate (B) as a first laminate, and a crack formation process was performed using the laminate (B) to obtain a transfer laminate sheet (B). Further, the same operations as in Example 1 were performed to obtain a patterned transfer product. The evaluation results are shown in Table 1.

[0136] Example 3 In Example 1, the cholesteric liquid crystal cured layer (CLC_G) produced in Production Example 3 was used as the liquid crystal cured layer, and the adhesive film was "H120" manufactured by Nichiei Shinka Co., Ltd. (a film comprising an adhesive layer (1) (thickness 20 μm) containing an acrylic adhesive and a transparent PET layer (thickness 75 μm)). Except for the above, the same operation as in Example 1 was performed to form a laminate (C). Furthermore, the liquid crystal cured layer (CLC_R) produced in Production Example 2 was bonded to the liquid crystal cured layer (CLC_G) side of this laminate (C) using a UV adhesive ("UVX6298" manufactured by Toa Gosei Co., Ltd.), and then the support substrate film was peeled off to obtain a laminate (C') as a first laminate having a layer structure of the liquid crystal cured layer (CLC_R) / UV adhesive layer / liquid crystal cured layer (CLC_G) / adhesive layer (1) / transparent PET layer. A crack formation process was performed using the laminate (C') to obtain a transfer laminate sheet (C'). Further, a patterned transfer product was obtained by carrying out the same procedure as in Example 1. The evaluation results are shown in Table 1.

[0137] Example 4 In Example 3, the adhesive film was "RC611" manufactured by Nichiei Shinka Co., Ltd. (a film having an adhesive layer (1) (thickness 20 μm) containing an acrylic adhesive and a transparent PET layer (thickness 75 μm). Except for the above, the same operation as in Example 3 was performed to obtain a laminate (D) having a layer structure of liquid crystal cured layer (CLC_R) / UV adhesive layer / liquid crystal cured layer (CLC_G) / adhesive layer (1) / transparent PET layer. Furthermore, the liquid crystal cured layer (CLC_B) produced in Production Example 4 was attached to the liquid crystal cured layer (CLC_R) side of this laminate (D) using a UV adhesive ("UVX6298" manufactured by Toa Gosei Co., Ltd.), and then the support substrate film was peeled off to obtain a laminate (D') as a first laminate having a layer structure of liquid crystal cured layer (CLC_B) / UV adhesive layer / liquid crystal cured layer (CLC_R) / UV adhesive layer / liquid crystal cured layer (CLC_G) / adhesive layer (1) / transparent PET layer. A crack formation process was performed using the laminate (D') to obtain a transfer laminate sheet (D'). Furthermore, the same operation as in Example 1 was performed to obtain a patterned transfer product. The evaluation results are shown in Table 1.

[0138] Comparative Example 1 In Example 1, a crack formation step was carried out using a multilayer film (laminate (E), peel strength 0.01 N / 25 mm) having a layer structure of a support substrate film / cured liquid crystal layer (CLC_W) produced in Production Example 1 instead of the laminate (A), to obtain a transfer laminate sheet (E). Further, the same operation as in Example 1 was carried out to obtain a patterned transfer product. The evaluation results are shown in Table 1.

[0139] Comparative Example 2 In Production Example 1, a 5 wt % aqueous polyvinyl alcohol solution ("MP203" manufactured by Kuraray Co., Ltd.) was applied onto the support substrate film, followed by drying at 100°C for 2 minutes. A 0.1 μm thick polyvinyl alcohol (PVA) layer was formed on the support substrate film as an alignment film, and an alignment substrate having a layer structure of support substrate film / PVA layer was obtained. The same procedure as in Production Example 1 was performed, except that the resulting alignment substrate was used instead of the support substrate film and the surface of the PVA layer of the alignment substrate was subjected to a rubbing treatment, to obtain a multilayer film comprising a support substrate film, a PVA layer, and a cured cholesteric liquid crystal layer. A transfer laminate sheet was obtained in the same manner as in Example 1, except that the resulting multilayer film was used, and a transfer product was obtained. The evaluation results are shown in Table 1. The peel strength between the polyvinyl alcohol layer and the cured liquid crystal layer was measured using the above-mentioned method and was 0.05 N / 25 m.

[0140] <Evaluation Results of Examples 1 to 4 and Comparative Examples 1 and 2> The evaluation results are shown in Table 1. The abbreviations in Table 1 have the following meanings. "CLC layer": cured cholesteric liquid crystal layer included in the transfer laminate sheet "W": broadband reflective cured cholesteric liquid crystal layer (CLC_W) "G": green reflective cured cholesteric liquid crystal layer (CLC_G) "G / R": green reflective cured cholesteric liquid crystal layer (CLC_G) and red reflective cholesteric liquid crystal layer (CLC_R) "B / G / R": blue reflective cured cholesteric liquid crystal layer (CLC_B), green reflective cholesteric liquid crystal layer (CLC_G), and red reflective cholesteric liquid crystal layer (CLC_R) "Adhesive layer peel strength": peel strength between the adhesive layer (adhesive layer (1)) and the cured cholesteric liquid crystal layer

[0141]

[0142] From the above results, in the transfer laminate sheets according to Comparative Examples 1 and 2, which do not have an adhesive layer (1) as an adhesive layer between the release base layer (transparent PET layer) and the cured cholesteric liquid crystal layer (CLC_W) as a dividing layer, chipping was observed both in the outline of the pattern shape and inside the pattern outline, and it can be seen that the clarity was inferior compared to the Examples. On the other hand, in the transfer laminate sheets according to the Examples, which have an adhesive layer (1) as an adhesive layer between the release base layer (transparent PET layer) and the cured cholesteric liquid crystal layer as a dividing layer, chipping was reduced compared to Comparative Examples 1 and 2, and it was found that the clarity was improved.

[0143] Examples 5 to 9 In Examples 5 to 9 shown below, a transfer laminate sheet having a retardation layer was produced, and it was demonstrated that the transferred product was useful as an identification medium.

[0144] <Evaluation Method> <Observation with Circularly Polarized Viewer and Polarized Sunglasses> Observation with Circularly Polarized Viewer: When the transfer was observed from the front through a circularly polarized viewer, whether the appearance differed from that observed with the naked eye and whether the pattern was discernible was evaluated according to the following criteria. The circularly polarized viewer was one in which the cholesteric liquid crystal cured layer (CLC_W) of the multilayer film produced in Production Example 1 was transferred onto a glass plate with an adhesive. Difference: There is a difference in appearance between observation with the naked eye and observation with the circularly polarized viewer, or the pattern is discernible when observed with the circularly polarized viewer. No difference: There is no difference in appearance between observation with the naked eye and observation with the circularly polarized viewer, and the pattern cannot be discerned when observed with the circularly polarized viewer.

[0145] Observation with polarized sunglasses: When an observer wore polarized sunglasses equipped with a linear polarizer and observed the transfer from the front, the observer evaluated whether the appearance differed from that observed with the naked eye and whether the pattern was discernible according to the following criteria: Large difference: There was a difference in appearance between observation with the naked eye and observation with polarized sunglasses, and the pattern was clearly discernible when observed with polarized sunglasses. Difference: There was a difference in appearance between observation with the naked eye and observation with polarized sunglasses, or the pattern was discernible when observed with polarized sunglasses. No difference: There was no difference in appearance between observation with the naked eye and observation with polarized sunglasses, and the pattern was not discernible when observed with polarized sunglasses.

[0146] Example 5 The transfer product prepared in Example 1 was evaluated by the above observation method. The evaluation results are shown in Table 2.

[0147] Example 6 An adhesive film ("PET75-H109" manufactured by Nichiei Shinka Co., Ltd.) was attached to the surface of the liquid crystal cured layer of the multilayer film containing the liquid crystal cured layer having a phase difference of λ / 4. After that, the support substrate film was peeled off, and a laminate (F) having a layer structure of a liquid crystal cured layer / adhesive layer (1) / transparent PET layer having a phase difference of λ / 4 was prepared. In the obtained laminate (F), the peel strength between the liquid crystal cured layer and the adhesive layer was measured and found to be 0.15 N / 25 mm. The cholesteric liquid crystal cured layer (CLC_W) prepared in Production Example 1 was further laminated to the laminate (F) with a UV adhesive ("UVX6298" manufactured by Toa Gosei Co., Ltd.), and then the support substrate film was peeled off. A laminate (F') having a layer structure of a cholesteric liquid crystal cured layer (CLC_W) / UV adhesive layer / λ / 4 liquid crystal cured layer / adhesive layer (1) / transparent PET layer having a phase difference of 4 was prepared. Using laminate (F') instead of laminate (A), the same operations as in Example 1 from the crack formation step onwards were carried out to obtain a transfer laminate sheet. The transfer laminate sheet had multiple optical layers, including a cholesteric liquid crystal cured layer (CLC_W) and a retardation layer (a liquid crystal cured layer having a retardation of λ / 4) as multiple small fragment layers contained in the dividing layer directly connected to the adhesive layer (1). A transfer was obtained using the obtained transfer laminate sheet. The obtained transfer was evaluated using the above-mentioned observation method. The evaluation results are shown in Table 2.

[0148] <Example 7> In Example 6, instead of the multilayer film produced in Production Example 5, a multilayer film containing a liquid crystal cured layer having a λ / 4 pattern retardation produced in Production Example 6 was used. In the obtained laminate, the peel strength between the liquid crystal cured layer having a λ / 4 pattern retardation and the adhesive layer was measured and found to be 0.14 N / 25 mm. Except for the above, the same operation as in Example 6 was performed to obtain a transfer laminate sheet. The transfer laminate sheet was provided with an optical layer containing a cholesteric liquid crystal cured layer (CLC_W) and a retardation layer (a liquid crystal cured layer having a λ / 4 retardation) as a plurality of small fragment layers contained in the dividing layer directly connected to the adhesive layer (1), and a small fragment layer containing a cholesteric liquid crystal cured layer (CLC_W) and an isotropic layer. A transfer product was obtained using the obtained transfer laminate sheet. The obtained transfer product was evaluated using the above observation method. The evaluation results are shown in Table 2.

[0149] <Example 8> In Example 6, a multilayer film containing a cured liquid crystal layer having a λ / 2 pattern retardation produced in Production Example 7 was used instead of the multilayer film produced in Production Example 5. In the obtained laminate, the peel strength between the cured liquid crystal layer having a λ / 2 pattern retardation and the adhesive layer was measured and found to be 0.15 N / 25 mm. Except for the above, the same operation as in Example 6 was performed to obtain a transfer laminate sheet. The transfer laminate sheet was provided with an optical layer containing a cholesteric liquid crystal cured layer (CLC_W) and a retardation layer (a cured liquid crystal layer having a λ / 2 retardation) as a plurality of small fragment layers contained in the dividing layer directly connected to the adhesive layer (1), and a small fragment layer containing a cholesteric liquid crystal cured layer (CLC_W) and an isotropic layer. A transfer product was obtained using the obtained transfer laminate sheet. The obtained transfer product was evaluated using the above observation method. The evaluation results are shown in Table 2.

[0150] <Example 9> After lambda / 2 pattern retardation produced in Production Example 7 was attached to the surface of the liquid crystal cured layer of the liquid crystal cured layer (Nichiei Shinka Co., Ltd. "PET75-H109": a film comprising an adhesive layer (1) and a transparent PET layer), the support substrate film was peeled off, and a laminate (G) having a layer structure of a liquid crystal cured layer / adhesive layer (1) / transparent PET layer having a pattern retardation of lambda / 2 was prepared. After laminating a multilayer film having a liquid crystal cured layer having a retardation of lambda / 4 produced in Production Example 5 to the laminate (G) with a UV adhesive (Toa Gosei Co., Ltd. "UVX6298"), the support substrate film was peeled off, (lambda / 4 phase retardation of the liquid crystal cured layer) / UV adhesive layer / (lambda / 2 pattern retardation of the liquid crystal cured layer) / adhesive layer (1) / transparent PET layer A laminate (G ') having a layer structure was prepared. Further, on the surface of the liquid crystal cured layer having a phase difference of λ / 4 of the laminate (G '), a multilayer film comprising the cholesteric liquid crystal cured layer (CLC_W) produced in Production Example 1 was laminated with a UV adhesive, and the support substrate film was peeled off, cholesteric liquid crystal cured layer (CLC_W) / UV adhesive layer / (liquid crystal cured layer having a phase difference of λ / 4) / UV adhesive layer / (liquid crystal cured layer having a pattern phase difference of λ / 2) / adhesive layer (1) / transparent PET layer having a layer structure (G '') was created. Using the laminate (G '') instead of the laminate (A), the same operations as in Example 1 after the crack formation process were performed to obtain a transfer laminate sheet. The transfer laminate sheet has a plurality of small fragment layers contained in the dividing layer directly connected to the adhesive layer (1), including a cholesteric liquid crystal cured layer (CLC_W), a retardation layer (a liquid crystal cured layer having a phase difference of λ / 4), and a retardation layer (a liquid crystal cured layer having a phase difference of λ / 2) in this order. Also included was an optical layer including a cholesteric liquid crystal cured layer (CLC_W), a retardation layer (a liquid crystal cured layer having a phase difference of λ / 4), and an isotropic layer in this order. A transfer was obtained using the obtained transfer laminate sheet. The obtained transfer was evaluated using the above-mentioned observation method. The evaluation results are shown in Table 2.

[0151] <Evaluation Results of Examples 5 to 9> The evaluation results are shown in Table 2. The abbreviations in Table 2 have the following meanings. "λ / 4": cured liquid crystal layer having a λ / 4 retardation produced in Production Example 5. "λ / 4 pattern": cured liquid crystal layer having a λ / 4 pattern retardation produced in Production Example 6. "λ / 2 pattern": cured liquid crystal layer having a λ / 2 pattern retardation produced in Production Example 7. "λ / 2 pattern + λ / 4": cured liquid crystal layer having a λ / 2 pattern retardation and a cured liquid crystal layer having a λ / 4 retardation.

[0152]

[0153] From the above results, it can be seen that transfers made using the transfer laminate sheets of Examples 6 to 9, in which the small fragment layer has a retardation layer, can identify patterns that cannot be identified by naked eye observation when observed using a circularly polarized viewer or polarized sunglasses.

[0154] 100: Transfer laminate sheet 110: Peel-off substrate layer 120: Adhesive layer 120D: Main surface 120U: Main surface 130: Dividing layer 141: Cured cholesteric liquid crystal layer 150: Crack 200: Transfer laminate sheet 230: Dividing layer 240: Optical layer 241: Cured cholesteric liquid crystal layer 242: Retardation layer 250: Crack 300: Transfer laminate sheet 330: Dividing layer 340a, 340b: Optical layer 341: Cured cholesteric liquid crystal layer 342, 343: Retardation layer 344: Isotropic layer

Claims

1. A transfer laminate sheet comprising, in that order, a release substrate layer, an adhesive layer, and a dividing layer directly adjacent to the adhesive layer, the dividing layer comprising a cholesteric liquid crystal cured layer and a plurality of small fragment layers divided by cracks.

2. The transfer laminate sheet according to claim 1, wherein the peel strength between the adhesive layer and the dividing layer is 0.1 N / 25 mm or more and 2 N / 25 mm or less.

3. The transfer laminate sheet according to claim 1, wherein the adhesive layer is provided on the entire surface of the release base layer.

4. The transfer laminate sheet according to claim 1, which is long.

5. The transfer laminate sheet according to claim 1, wherein the adhesive layer is a layer of pressure-sensitive adhesive containing one or more types selected from the group consisting of acrylic pressure-sensitive adhesives, urethane pressure-sensitive adhesives, rubber pressure-sensitive adhesives, silicone pressure-sensitive adhesives, polyester pressure-sensitive adhesives, and ethylene vinyl acetate pressure-sensitive adhesives.

6. The transfer laminate sheet according to claim 1, wherein a part or all of the plurality of small fragment layers included in the dividing layer are optical layers including the cholesteric liquid crystal cured layer and a retardation layer.

7. The transfer laminate sheet according to claim 6, wherein the retardation layer included in the optical layer is a λ / 4 plate.

8. The transfer laminate sheet described in claim 6, wherein the multiple small fragment layers contained in the dividing layer include two types of optical layers, and the absolute value of the difference between the in-plane retardation values ​​of the two types of optical layers is (λ / 2-60 nm) or more and (λ / 2+60 nm) or less at a measurement wavelength λ.

9. The transfer laminate sheet according to claim 6, wherein the optical layer is disposed on the adhesive layer in a pattern.

10. A method for producing a transfer laminate sheet according to any one of claims 1 to 9, comprising: a step (1) of preparing a first laminate including, in this order, the release base layer, the adhesive layer, and a layer (A) directly on the adhesive layer and including the cholesteric liquid crystal cured layer; and a step (2) of forming cracks in the layer (A) included in the first laminate to divide the layer (A) and form a plurality of small fragment layers.

Citation Information

Patent Citations

  • Production of liquid crystal polymer film

    JP1996278491A

  • Manufacturing method of patch transfer medium, and patch transfer medium

    JP2012179778A

  • Optical laminate, method for manufacturing optical laminate, and transfer material for manufacturing optical laminate

    JP2016016538A

  • Liquid crystal cured layer transfer seal, liquid crystal cured layer transfer matter, and method for assessing authenticity of liquid crystal cured layer transfer seal

    WO2021079815A1

  • Display medium, method for manufacturing same, and display article

    WO2021172567A1