Copolymer, positive resist composition, and resist pattern formation method

The use of a copolymer with specific monomer units in a positive resist composition addresses the limitations of conventional resists by expanding exposure margins and improving pattern shapes, facilitating advanced semiconductor manufacturing.

WO2024203557A1PCT designated stage expired Publication Date: 2024-10-03ZEON CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010605
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional main chain cleavage type positive resists in semiconductor manufacturing have limited exposure margins and do not form resist patterns with optimal shapes, necessitating improvements for higher integration and better pattern quality.

Method used

A copolymer comprising specific monomer units, including a monomer unit with a -2,2,2-trifluoroethyl group and an α-methylstyrene unit, is used to expand the exposure margin and improve the shape of resist patterns, with the copolymer being formulated into a positive resist composition and processed using a method involving exposure and development to form well-defined patterns.

Benefits of technology

The copolymer-based positive resist composition enhances the exposure margin and pattern shape, enabling the formation of high-quality resist patterns suitable for advanced semiconductor manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010605_03102024_PF_FP_ABST
    Figure JP2024010605_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a copolymer and a positive resist composition, which make it possible to form a resist pattern that has a wide light exposure margin and a favorable shape. A copolymer according to the present invention is characterized by comprising a monomer unit (I) represented by formula (I), a monomer unit (II) represented by formula (II), and a monomer unit (III) represented by formula (III). In the formulae, R1 to R14 each represent a predetermined group, and p represents an integer of 0 to 5 (inclusive).
Need to check novelty before this filing date? Find Prior Art

Description

Copolymer, positive resist composition, and method for forming a resist pattern

[0001] The present invention relates to a copolymer, a positive resist composition, and a method of forming a resist pattern.

[0002] Conventionally, in fields such as semiconductor manufacturing, polymers whose main chains are scissed and whose solubility in a developer is increased by irradiation with ionizing radiation such as electron beams and extreme ultraviolet (EUV) radiation, or non-ionizing radiation including short-wavelength light such as ultraviolet radiation (hereinafter, sometimes collectively referred to as "ionizing radiation, etc.") have been used as main-chain scission-type positive resists. Specifically, for example, Patent Document 1 discloses a main-chain scission-type positive resist capable of efficiently forming fine resist patterns with high resolution, which contains a copolymer having α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units and 4-methyl-α-methylstyrene units or α-methylstyrene units and having a weight-average molecular weight of more than 100,000.

[0003] International Publication No. 2022 / 070928

[0004] In recent years, due to demands for higher integration of semiconductor integrated circuits, etc., main chain scission type positive resists are required to have a wide exposure margin (i.e., a wide tolerance for the amount of exposure in the exposure step). Main chain scission type positive resists are also required to have an excellent resist pattern shape formed through the exposure step and development treatment (development step) using a developer. However, the above-mentioned conventional positive resists have room for improvement in terms of widening the exposure margin while providing a good resist pattern shape.

[0005] Therefore, an object of the present invention is to provide a copolymer and a positive resist composition that are capable of forming a resist pattern with a wide exposure margin and a good shape, and also to provide a method of forming a resist pattern that is capable of forming a resist pattern with a wide exposure margin and a good shape.

[0006] The present inventors have conducted extensive research to achieve the above object, and have newly discovered that by using a copolymer containing three specific monomer units, it is possible to form a resist pattern with a good shape while widening the exposure margin of the resist, and have completed the present invention.

[0007] That is, the object of the present invention is to advantageously solve the above-mentioned problems, and the present invention provides: [1] a compound represented by the following formula (I): (In formula (I), R 1 is a halogen atom or an alkyl group substituted with a halogen atom, and R 2 is an organic group having a fluorine atom, and R 3 and R 4 are hydrogen atoms, halogen atoms, unsubstituted alkyl groups or alkyl groups substituted with halogen atoms, and may be the same or different from each other), and a monomer unit (I) represented by the following formula (II): (In formula (II), R 5 is a halogen atom or an alkyl group substituted with a halogen atom, and R 6 , R 7 and R 8 are hydrogen atoms or aliphatic groups which may have a substituent and do not have a fluorine atom, and may be the same or different from each other, R 6 , R 7 and R 8 may form a ring structure together with the carbon atom to which they are attached, and R 9 and R 10 are hydrogen atoms or unsubstituted alkyl groups, and may be the same or different from each other.) and a monomer unit (II) represented by the following formula (III): (In formula (III), R 11 and R 12 are hydrogen atoms or unsubstituted alkyl groups, which may be the same or different from each other, and R 13 is an alkyl group which may have a substituent, and R 14is a halogen atom or an organic group, and p is an integer of 0 or more and 5 or less. In this way, by using a copolymer containing the above-mentioned predetermined monomer units (I) to (III), it is possible to form a resist pattern having a good shape while increasing the exposure margin of the obtained resist.

[0008] [2] In the copolymer of [1] above, the R 2 is preferably a group represented by L-Ar (wherein L is a divalent linking group having a fluorine atom, and Ar is an aromatic ring group which may have a substituent). 2 When is a group having the above-mentioned predetermined structure, the sensitivity of the copolymer to ionizing radiation and the like can be improved.

[0009] [3] In the copolymer of [1] or [2] above, the R 6 , the R 7 and the R 8 is preferably a hydrogen atom or an aliphatic group having 1 to 10 carbon atoms and no fluorine atom, which may have a substituent. 6 , R 7 and R 8 When is a hydrogen atom or one of the above-mentioned specific aliphatic groups, it is possible to further widen the exposure margin and form a resist pattern with a better shape.

[0010] [4] In any of the copolymers [1] to [3] above, the proportion of the monomer unit (II) is preferably less than 30 mol %. Thus, if the proportion of the monomer unit (II) in the copolymer is less than the above upper limit, it is possible to further widen the exposure margin and form a resist pattern with a better shape. In the present invention, the proportion of the monomer unit in the copolymer can be measured by the method described in the Examples.

[0011] Another object of the present invention is to advantageously solve the above-mentioned problems, and the present invention provides [5] a positive resist composition comprising the copolymer of any one of [1] to [4] above and a solvent. This positive resist composition makes it possible to form a resist pattern with an even better shape while further expanding the exposure margin.

[0012] Another object of the present invention is to advantageously solve the above-mentioned problems, and the present invention provides [6] a method of forming a resist pattern, comprising the steps of forming a resist film using the positive resist composition according to the above [5], exposing the resist film, and developing the exposed resist film. By using this method of forming a resist pattern, it is possible to form a resist pattern having a good shape with a wide exposure margin.

[0013] [7] In the method for forming a resist pattern according to [6] above, the development is preferably carried out using an alcohol-based solvent. By using an alcohol-based solvent for development, a resist pattern having a better shape can be formed.

[0014] According to the present invention, it is possible to provide a copolymer and a positive resist composition which are capable of forming a resist pattern which has a wide exposure margin and a good shape, and also to provide a method of forming a resist pattern which is capable of forming a resist pattern which has a wide exposure margin and a good shape.

[0015] Embodiments of the present invention are described in detail below. The copolymer of the present invention can be used, for example, to produce a main chain scission-type positive resist composition in which the main chain is scissed by ionizing radiation or the like, resulting in a lower molecular weight, and can be suitably used in the production of the positive resist composition of the present invention. The positive resist composition of the present invention comprises the copolymer of the present invention, and can be suitably used, for example, in the method of forming a resist pattern of the present invention. The method of forming a resist pattern of the present invention can be suitably used, for example, when forming a resist pattern in the production processes of printed circuit boards such as build-up boards, semiconductors, photomasks, molds, etc.

[0016] (Copolymer) The copolymer of the present invention is (In formula (I), R 1 is a halogen atom or an alkyl group substituted with a halogen atom, and R 2 is an organic group having a fluorine atom, and R 3 and R 4 are hydrogen atoms, halogen atoms, unsubstituted alkyl groups or alkyl groups substituted with halogen atoms, and may be the same or different from each other), and a monomer unit (I) represented by the following formula (II): (In formula (II), R 5 is a halogen atom or an alkyl group substituted with a halogen atom, and R 6 , R 7 and R 8 are hydrogen atoms or optionally substituted aliphatic groups not containing fluorine atoms, and may be the same or different from each other; R 6 , R 7 and R 8 may form a ring structure together with the carbon atom to which they are attached, and R 9 and R 10 are hydrogen atoms or unsubstituted alkyl groups, and may be the same or different from each other.) and a monomer unit (II) represented by the following formula (III): (In formula (III), R 11 and R 12 are hydrogen atoms or unsubstituted alkyl groups, which may be the same or different from each other, and R 13 is an alkyl group which may have a substituent, and R 14 is a halogen atom or an organic group, and p is an integer of 0 or more and 5 or less.

[0017] The copolymer of the present invention may contain other monomer units besides the monomer units (I) to (III). However, the proportion of the monomer units (I) to (III) in total of all the monomer units (100 mol%) constituting the copolymer is preferably 90 mol% or more, more preferably 100 mol% (i.e., the copolymer is composed of the monomer units (I) to (III)). Furthermore, the copolymer of the present invention is not particularly limited as long as it contains the monomer units (I) to (III), and may be any of a random copolymer, a block copolymer, a ternary alternating copolymer, and the like. In the present invention, a ternary alternating copolymer is an alternating copolymer in which the monomer unit (I) or the monomer unit (II) is copolymerized between the monomer units (III). That is, schematically, the individual monomer units are bonded as "-(III)-(I)-(III)-(II)-(III)-".

[0018] The copolymer of the present invention contains the predetermined monomer units (I) to (III), and when irradiated with ionizing radiation or the like, the main chain of the copolymer is effectively cleaved only in the irradiated portion, resulting in a low molecular weight. The low-molecular-weight component then dissolves well in a developer. Furthermore, the reason why the copolymer of the present invention contains the predetermined monomer units (I) to (III) is able to form a resist pattern with a good shape while widening the exposure margin of the resulting resist is not entirely clear, but is presumed to be as follows. That is, by containing the monomer units (I), (II), and (III), which have different solubilities in a developer, it is possible to control the solubility in the developer, and therefore it is presumed that the copolymer can form a resist pattern with a good shape while widening the exposure margin.

[0019] <Monomer Unit (I)> The monomer unit (I) contained in the copolymer of the present invention is a monomer unit represented by the following formula (a): (In formula (a), R 1 ~R 4 has the same meaning as formula (I).

[0020] Here, R in formula (I) and formula (a) 1 , R 3 , R4 The halogen atoms that can constitute R are not particularly limited, and examples thereof include a chlorine atom, a fluorine atom, a bromine atom, and an iodine atom. 1 , R 3 , R 4 The alkyl group substituted with a halogen atom that can constitute the above group is not particularly limited, and examples thereof include groups having a structure in which some or all of the hydrogen atoms in the alkyl group are substituted with the above halogen atoms. 3 , R 4 The unsubstituted alkyl group that can constitute R is not particularly limited, and examples thereof include unsubstituted alkyl groups having 1 to 10 carbon atoms. 3 , R 4 The unsubstituted alkyl group that can constitute the above is preferably a methyl group or an ethyl group.

[0021] From the viewpoint of improving the scission property of the main chain of the copolymer when irradiated with exposure light and increasing the efficiency of forming a resist pattern, R 1 is preferably a chlorine atom, a fluorine atom, or an alkyl group having 1 to 5 carbon atoms substituted with a fluorine atom, more preferably a chlorine atom, a fluorine atom, or a perfluoromethyl group, further preferably a chlorine atom or a fluorine atom, and particularly preferably a chlorine atom. 1 The monomer (a) in which R is a chlorine atom has excellent polymerizability, and 1 The copolymer having the monomer unit (I) in which is a chlorine atom is also advantageous in that it can be easily prepared.

[0022] Furthermore, from the viewpoint of improving the scission property of the polymer main chain when irradiated with exposure light and increasing the efficiency of resist pattern formation, it is preferable that R 3 and R 4 are each preferably a hydrogen atom or an unsubstituted alkyl group, more preferably a hydrogen atom or an unsubstituted alkyl group having 1 to 5 carbon atoms, and even more preferably a hydrogen atom.

[0023] R in formula (I) and formula (a) 2 The "organic group having a fluorine atom" that can constitute the above formula is not particularly limited, and examples thereof include a fluoroalkyl group, a fluoroalkoxyalkyl group, a fluoroalkoxyalkenyl group, and a group represented by L-Ar (wherein L is a divalent linking group having a fluorine atom, and Ar is an aromatic ring group which may have a substituent). Here, from the viewpoint of improving the scission property of the main chain of the copolymer when irradiated with ionizing radiation or the like and thereby increasing the efficiency of forming a resist pattern, R 2 The number of fluorine atoms in R is preferably 1 or more and 11 or less. 2 The number of fluorine atoms in R is more preferably 3 or more, more preferably 4 or more, and is preferably 9 or less. 2 The number of carbon atoms in the group R in formula (I) and formula (a) can be 1 or more and 12 or less. In particular, from the viewpoint of improving the sensitivity of the copolymer to ionizing radiation and the like, 2 is more preferably a group represented by L-Ar.

[0024] R 2Examples of the fluoroalkyl group constituting the formula (I) include a monofluoromethyl group (one fluorine atom, one carbon atom), a monofluoroethyl group (one fluorine atom, two carbon atoms), a 2,2-difluoroethyl group (two fluorine atoms, two carbon atoms), a 2,2,2-trifluoromethyl group (three fluorine atoms, one carbon atom), a 2,2,2-trifluoroethyl group (three fluorine atoms, two carbon atoms), a 2,2,3,3,3-pentafluoropropyl group (five fluorine atoms, three carbon atoms), a 3,3,4,4,4-pentafluorobutyl group (five fluorine atoms, four carbon atoms), a 2-(perfluorobutyl)ethyl group (nine fluorine atoms, six carbon atoms), a 1H,1H,3H-tetrafluoropropyl group (four fluorine atoms, three carbon atoms), a 1H,1H,5H-octafluoropentyl group (four fluorine atoms, three ... R is preferably a 1,2,3,3-pentafluoropropyl group, a 1H-1-(trifluoromethyl)trifluoroethyl group (having 8 fluorine atoms and 5 carbon atoms), a 1H,1H,3H-hexafluorobutyl group (having 6 fluorine atoms and 4 carbon atoms), a 2,2,3,3,4,4,4-heptafluorobutyl group (having 7 fluorine atoms and 4 carbon atoms), or a 1,2,2,2-tetrafluoro-1-(trifluoromethyl)ethyl group (having 7 fluorine atoms and 3 carbon atoms), and more preferably a 2,2,3,3,3-pentafluoropropyl group, a 1H-1-(trifluoromethyl)trifluoroethyl group, a 1H,1H,3H-hexafluorobutyl group, a 2,2,3,3,4,4,4-heptafluorobutyl group, or a 1,2,2,2-tetrafluoro-1-(trifluoromethyl)ethyl group. 2 The fluoroalkoxyalkyl group constituting R is preferably, for example, a pentafluoromethoxymethyl group (having 5 fluorine atoms and 2 carbon atoms), a pentafluoroethoxymethyl group (having 5 fluorine atoms and 3 carbon atoms), or a pentafluoroethoxyethyl group (having 5 fluorine atoms and 4 carbon atoms). 2 The fluoroalkoxyalkenyl group constituting the formula (I) is preferably, for example, a pentafluoroethoxyvinyl group (having 5 fluorine atoms and 4 carbon atoms).

[0025] Examples of the divalent linking group having a fluorine atom that can constitute L in the group represented by L-Ar include a divalent chain alkylene group having a fluorine atom and having 1 to 5 carbon atoms. Specific examples of the divalent linking group having a fluorine atom include a trifluoromethylmethylene group, a pentafluoroethylmethylene group, and a bis(trifluoromethyl)methylene group. Among these, a pentafluoroethylmethylene group and a bis(trifluoromethyl)methylene group are preferred, and a bis(trifluoromethyl)methylene group is more preferred.

[0026] The number of fluorine atoms in L is preferably 3 or more, more preferably 4 or more, and even more preferably 5 or more, and is preferably 11 or less, and more preferably 9 or less. When the number of fluorine atoms in L is equal to or greater than the above-mentioned lower limit, the sensitivity to exposure light can be further improved. On the other hand, when the number of fluorine atoms in L is equal to or less than the above-mentioned upper limit, the production efficiency of the copolymer can be improved.

[0027] Furthermore, examples of Ar in the group represented by L-Ar include aromatic hydrocarbon ring groups which may have a substituent and aromatic heterocyclic groups which may have a substituent.

[0028] The aromatic hydrocarbon ring group is not particularly limited, and examples thereof include a benzene ring group, a biphenyl ring group, a naphthalene ring group, an azulene ring group, an anthracene ring group, a phenanthrene ring group, a pyrene ring group, a chrysene ring group, a naphthacene ring group, a triphenylene ring group, an o-terphenyl ring group, an m-terphenyl ring group, a p-terphenyl ring group, an acenaphthene ring group, a coronene ring group, a fluorene ring group, a fluoranthrene ring group, a pentacene ring group, a perylene ring group, a pentaphene ring group, a picene ring group, and a pyranthrene ring group.

[0029] Furthermore, the aromatic heterocyclic group is not particularly limited, and examples thereof include a furan ring group, a thiophene ring group, a pyridine ring group, a pyridazine ring group, a pyrimidine ring group, a pyrazine ring group, a triazine ring group, an oxadiazole ring group, a triazole ring group, an imidazole ring group, a pyrazole ring group, a thiazole ring group, an indole ring group, a benzimidazole ring group, a benzothiazole ring group, a benzoxazole ring group, a quinoxaline ring group, a quinazoline ring group, a phthalazine ring group, a benzofuran ring group, a dibenzofuran ring group, a benzothiophene ring group, a dibenzothiophene ring group, and a carbazole ring group.

[0030] Furthermore, the substituent that Ar may have is not particularly limited, and examples thereof include an alkyl group, a fluorine atom, and a fluoroalkyl group. Examples of the alkyl group that Ar may have as a substituent include a chain alkyl group having 1 to 6 carbon atoms, such as a methyl group, an ethyl group, a propyl group, an n-butyl group, and an isobutyl group. Examples of the fluoroalkyl group that Ar may have as a substituent include a fluoroalkyl group having 1 to 5 carbon atoms, such as a trifluoromethyl group, a trifluoroethyl group, and a pentafluoropropyl group.

[0031] Among these, from the viewpoint of improving the sensitivity to exposure light, Ar is preferably an aromatic hydrocarbon ring group which may have a substituent, more preferably an unsubstituted aromatic hydrocarbon ring group, and even more preferably a benzene ring group (phenyl group).

[0032] From the viewpoint of improving the sensitivity to exposure light, in formula (I) and formula (a), R 2 is preferably a group represented by L-Ar, and in formula (I) and formula (a), R 1 is a chlorine atom, and R 3 and R 4 is a hydrogen atom, and R 2 is more preferably a group represented by L-Ar.

[0033] The monomer (a) represented by the above formula (a) capable of forming the monomer unit (I) represented by the above formula (I) is not particularly limited, and examples thereof include monofluoromethyl α-chloroacrylate, monofluoroethyl α-chloroacrylate, 2,2-difluoroethyl α-chloroacrylate, 2,2,2-trifluoroethyl α-chloroacrylate, 2,2,3,3,3-pentafluoropropyl α-chloroacrylate, 3,3,4,4,4-pentafluorobutyl α-chloroacrylate, α-chloroacrylic acid ...3,3,4,4,4-pentafluorobutyl α-chloroacrylate, 3,3,4,4,4-pentafluorobutyl α-chloroacrylate, 3,3,4,4,4-pentafluorobutyl α-chloroacrylate, 3,3,4,4,4-pentafluorobutyl α-chloroacrylate, 3,3,4,4,4 α-chloroacrylic acid such as 2-(perfluorobutyl)ethyl, 1H,1H,3H-tetrafluoropropyl α-chloroacrylate, 1H,1H,5H-octafluoropentyl α-chloroacrylate, 1H-1-(trifluoromethyl)trifluoroethyl α-chloroacrylate, 1H,1H,3H-hexafluorobutyl α-chloroacrylate, 2,2,3,3,4,4,4-heptafluorobutyl α-chloroacrylate, and 1,2,2,2-tetrafluoro-1-(trifluoromethyl)ethyl α-chloroacrylate. Acrylic acid fluoroalkyl esters: 2,2,2-trifluoroethyl α-fluoroacrylate, 2,2,3,3,3-pentafluoropropyl α-fluoroacrylate, 3,3,4,4,4-pentafluorobutyl α-fluoroacrylate, 2-(perfluorobutyl)ethyl α-fluoroacrylate, 1H,1H,3H-tetrafluoropropyl α-fluoroacrylate, 1H,1H,5H-octafluoropentyl α-fluoroacrylate, 1H-1-(trifluoromethyl)trifluoro α-fluoroacrylate α-Fluoroacrylic acid fluoroalkyl esters such as α-fluoroacrylic acid 1H,1H,3H-hexafluorobutyl ester, α-fluoroacrylic acid 2,2,3,3,4,4,4-heptafluorobutyl ester, and α-fluoroacrylic acid 1,2,2,2-tetrafluoro-1-(trifluoromethyl)ethyl ester; α-chloroacrylic acid fluoroalkoxyalkyl esters such as α-chloroacrylic acid pentafluoroethoxymethyl ester and α-chloroacrylic acid pentafluoroethoxyethyl ester;Examples of such fluoroalkoxyalkyl α-fluoroacrylates include α-fluoroacrylic acid pentafluoroethoxymethyl ester and α-fluoroacrylic acid pentafluoroethoxyethyl ester; α-chloroacrylic acid fluoroalkoxyalkenyl esters such as α-chloroacrylic acid pentafluoroethoxyvinyl ester; α-fluoroacrylic acid fluoroalkoxyalkenyl esters such as α-fluoroacrylic acid pentafluoroethoxyvinyl ester; and α-chloroacrylic acid-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl (ACAFPh). These may be used alone or in combination of two or more. Of these, α-chloroacrylic acid-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl (ACAFPh) is preferably used.

[0034] The proportion of the monomer units (I) in the copolymer is preferably 20 mol% or more, more preferably 30 mol% or more, and even more preferably 40 mol% or more, and is preferably 80 mol% or less, more preferably 70 mol% or less, and even more preferably 65 mol% or less, when the total amount of all the monomer units in the copolymer is taken as 100 mol%. If the proportion of the monomer units (I) in the copolymer is within the above range, when the total amount of all the monomer units in the copolymer is taken as 100 mol%, the sensitivity to ionizing radiation and the like can be increased.

[0035] <Monomer Unit (II)> The monomer unit (II) contained in the copolymer of the present invention is a monomer unit represented by the following formula (b): (In formula (b), R 5 ~R 10 is a structural unit derived from a monomer (b) represented by formula (II).

[0036] R in formula (II) and formula (b) 5The halogen atom or alkyl group substituted with a halogen atom that can constitute the formula (II) or (b) includes, but is not limited to, halogen atoms such as chlorine, fluorine, bromine, and iodine atoms; and groups having a structure in which some or all of the hydrogen atoms in an alkyl group are substituted with the above-mentioned halogen atoms. 5 The alkyl group of the alkyl group substituted with a halogen atom that can constitute R is not particularly limited, and examples thereof include unsubstituted alkyl groups having 1 to 5 carbon atoms. 5 The alkyl group of the alkyl group substituted with a halogen atom that can constitute the above is preferably a methyl group or an ethyl group.

[0037] R in formula (II) and formula (b) 6 , R 7 , R 8 The "optionally substituted aliphatic group having no fluorine atom" that can constitute R is not particularly limited as long as it does not contain a fluorine atom. From the viewpoint of further widening the exposure margin and forming a resist pattern with a better shape, 6 , R 7 , R 8 is preferably an optionally substituted aliphatic group having 1 to 10 carbon atoms and no fluorine atoms, and more preferably an optionally substituted aliphatic group having 1 to 8 carbon atoms and no fluorine atoms. The "number of carbon atoms" means the number of carbon atoms in the aliphatic group, not including the number of carbon atoms in the substituent.

[0038] The aliphatic group includes, but is not limited to, a chain aliphatic group and a cyclic aliphatic group. The chain aliphatic group includes, but is not limited to, an alkyl group, an alkenyl group, and the like. The alkyl group includes, but is not limited to, an alkyl group having 1 to 20 carbon atoms, specifically, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, and the like. Of these, a methyl group is preferred. The alkenyl group includes, but is not limited to, an alkenyl group having 1 to 20 carbon atoms, specifically, an ethenyl group (vinyl group), a propenyl group, an isopropenyl group, a butenyl group, an isobutenyl group, a tert-butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, an octenyl group, an isooctenyl group, a nonenyl group, and the like.

[0039] The cyclic aliphatic group may be either monocyclic or polycyclic, and examples of the monocyclic aliphatic group include a cycloalkyl group and a cycloalkenyl group. The cycloalkyl group is not particularly limited, and examples thereof include a cycloalkyl group having from 3 to 20 carbon atoms, specific examples of which include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cyclooctyl group, a cyclononyl group, and a cyclodecyl group. The cycloalkenyl group is not particularly limited, and examples thereof include a cycloalkenyl group having from 3 to 20 carbon atoms, specific examples of which include a 1-cyclopropyl group, a 1-cyclobutenyl group, a 1-cyclopentenyl group, a 1-cyclohexenyl group, a 1-cycloheptenyl group, and a 1-cyclooctenyl group.

[0040] The substituent is not particularly limited as long as it does not have a fluorine atom, and examples thereof include halogen atoms such as chlorine atoms, bromine atoms, and iodine atoms, amino groups, hydroxyl groups, carboxyl groups, sulfonyl groups, alkyl groups, cycloalkyl groups, alkylamino groups, dialkylamino groups, alkoxy groups, thiol groups, sulfide groups, and thioester groups. These alkyl groups, cycloalkyl groups, alkylamino groups, dialkylamino groups, and alkoxy groups may be further substituted with the halogen atoms, hydroxyl groups, amino groups, carboxyl groups, and sulfonyl groups. R 6 , R 7 , R 8 The number of the above-mentioned substituents in each of R is not particularly limited. 6 , R 7 or R 8 When a plurality of substituents are present in the formula (I), the plurality of substituents may be the same or different from each other.

[0041] The alkyl group as the substituent is not particularly limited, and R 6 , R 7 , R 8 Among these, alkyl groups having 1 to 4 carbon atoms, specifically, methyl, ethyl, n-propyl, isopropyl, isobutyl, and tert-butyl groups are preferred.

[0042] The cycloalkyl group as the substituent is not particularly limited, and R 6 , R 7 , R 8 Among these, a cycloalkyl group having 3 to 10 carbon atoms, such as a cyclohexyl group, is preferred.

[0043] Examples of the alkoxy group as the substituent include alkoxy groups having 1 to 12 carbon atoms, such as methoxy, ethoxy, and butoxy groups. Of these, methoxy is preferred.

[0044] Examples of the alkylamino group as the substituent include alkylamino groups having 1 to 12 carbon atoms, such as a methylamino group, an ethylamino group, an n-propylamino group, an i-propylamino group, a cyclopropylamino group, an n-butylamino group, an i-butylamino group, an s-butylamino group, a t-butylamino group, and a cyclobutylamino group.

[0045] Examples of the dialkylamino group as the substituent include dialkylamino groups having 2 to 12 carbon atoms, such as dimethylamino, diethylamino, dipropylamino, and dibutylamino.

[0046] R 6 , R 7 , and R 8 (More specifically, R 6 , R 7 , and R 8 The ring structure formed by combining the carbon atoms to which they are bonded with two or more of the following is not particularly limited, and may be either a monocyclic or polycyclic ring, as long as it does not contain a fluorine atom.

[0047] Examples of monocyclic ring structures include, but are not limited to, monocyclic aliphatic hydrocarbon rings such as a cyclopropane ring, a cyclobutane ring, a cyclopentane ring, a cyclohexane ring, a cycloheptane ring, a cyclooctane ring, a cyclononane ring, a cyclodecane ring, a cycloundecane ring, a cyclododecane ring, a cyclopentene ring, a cyclohexene ring, a cycloheptene ring, a cyclooctene ring, a cyclononene ring, a cyclodecene ring, and a cyclododecene ring; and monocyclic aliphatic heterocycles such as a lactone ring, a pyrrolidine ring, a tetrahydrothiophene ring, a piperidine ring, a tetrahydrothiopyran ring, a piperazine ring, a morpholine ring, and a dioxane ring. It is preferable that the monocyclic aliphatic heterocycle is not a pyranose ring or a furanose ring. Here, a heterocycle refers to a ring structure having one or more heteroatoms other than carbon, and may be a saturated or unsaturated ring. Examples of heteroatoms include, but are not limited to, a nitrogen atom, an oxygen atom, and a sulfur atom. Among these, the monocyclic ring structure is preferably an aliphatic hydrocarbon ring.

[0048] The polycyclic ring structure is not particularly limited, and may be a polycyclic structure in which two or more monocyclic rings are fused together, a polycyclic structure in which two or more rings are bonded to each other via a single bond or a linking group, a polycyclo ring structure with two or more rings, or a spiro ring structure. Here, examples of the monocyclic ring constituting the polycyclic structure include the monocyclic rings described above. Specific examples of the polycyclic structure include polycyclic aliphatic hydrocarbon rings such as a decalin ring, a hydrindane ring, an adamantane ring, a norbornane ring, a norbornene ring, an isobornane ring, a tricyclodecane ring, a tetracyclododecane ring, and a sterol ring; and polycyclic aliphatic heterocyclic rings such as a norbornane lactone ring, a 7-oxanorbornane ring, a 7-thionorbornane ring, and a 7-azanorbornane ring. Among these, an adamantane ring or a norbornane lactone ring is preferred.

[0049] These ring structures may have the above-mentioned substituents. When the ring structure has two or more substituents, the substituents may be the same or different from each other.

[0050] R in formula (II) and formula (b) 9 and R 10 The unsubstituted alkyl group that can constitute R is not particularly limited, and examples thereof include unsubstituted alkyl groups having 1 to 10 carbon atoms. 9 and R 10 The unsubstituted alkyl group that can constitute the above is preferably a methyl group or an ethyl group.

[0051] From the viewpoint of further widening the exposure margin and forming a resist pattern with a better shape, it is preferable that R 6 , R 7 and R 8 is preferably a hydrogen atom or an optionally substituted aliphatic group having 1 to 10 carbon atoms and no fluorine atom; R 5 is a chlorine atom, and R 6 , R 7 , R 8are hydrogen atoms or together with the carbon atoms to which they are attached form a polycyclic aliphatic hydrocarbon ring or a polycyclic aliphatic heterocycle, and R 9 and R 10 is more preferably a hydrogen atom; R 5 is a chlorine atom, and R 6 , R 7 , R 8 together with the carbon atoms to which they are attached form an adamantyl ring or a norbornane lactone ring, and R 9 and R 10 It is more preferable that is a hydrogen atom.

[0052] Specific examples of the monomer (b) represented by the above formula (b) which can form the monomer unit (II) represented by the above formula (II) include, but are not limited to, α-chloroacrylic acid alkyl esters such as methyl α-chloroacrylate, ethyl α-chloroacrylate, propyl α-chloroacrylate, butyl α-chloroacrylate, cyclohexyl α-chloroacrylate, and cycloheptyl α-chloroacrylate; methyl α-fluoroacrylate, ethyl α-fluoroacrylate, propyl α-fluoroacrylate, butyl α-fluoroacrylate, and cyclohexyl α-fluoroacrylate; and alkyl α-fluoroacrylates such as cycloheptyl α-fluoroacrylate; 1-adamantyl α-chloroacrylate; 1-adamantyl α-fluoroacrylate; 1-adamantylmethyl α-chloroacrylate; 1-adamantylmethyl α-fluoroacrylate; 2-adamantyl α-chloroacrylate; 2-adamantyl α-fluoroacrylate; α-chloroacrylic acid-norbornane lactone; α-fluoroacrylic acid-norbornane lactone; α-chloroacrylic acid-gamma-butyrolactone; and α-fluoroacrylic acid-gamma-butyrolactone. These may be used alone or in combination of two or more. Among these, from the viewpoint of forming a resist pattern having a better shape while further widening the exposure margin, the monomer (b) represented by formula (b) is preferably methyl α-chloroacrylate, 2-adamantyl α-chloroacrylate, α-chloroacrylic acid-norbornane lactone, or α-chloroacrylic acid-gamma butyrolactone.

[0053] That is, the copolymer preferably contains, as the monomer unit (II), an α-chloroacrylic acid methyl unit represented by the following formula (b-1), an α-chloroacrylic acid-2-adamantyl unit represented by the following formula (b-2), an α-chloroacrylic acid-norbornane lactone unit represented by the following formula (b-3), or an α-chloroacrylic acid-gamma butyrolactone unit represented by the following formula (b-4).

[0054] From the viewpoint of forming a resist pattern having a better shape while further widening the exposure margin, the proportion of the monomer unit (II) in the copolymer, when the total amount of all monomer units in the copolymer is taken as 100 mol %, is preferably 1.0 mol % or more, more preferably 2.0 mol % or more, preferably less than 30 mol %, more preferably 25 mol % or less, and even more preferably 20 mol % or less.

[0055] The total proportion of the monomer units (I) and (II) in the copolymer is preferably 30 mol % or more, more preferably 40 mol % or more, and is preferably 70 mol % or less, more preferably 65 mol % or less, when the total amount of all the monomer units in the copolymer is 100 mol %.

[0056] <Monomer Unit (III)> The monomer unit (III) is a monomer unit represented by the following formula (c): (In formula (c), R 11 ~R 14 and p is the same as in formula (III).

[0057] R in formula (III) and formula (c) 11 and R 12 The unsubstituted alkyl group that can constitute R is not particularly limited, and examples thereof include alkyl groups having 1 to 5 carbon atoms. 11 and R 12 The alkyl group that can constitute the group is preferably a methyl group or an ethyl group.

[0058] R in formula (III) and formula (c) 13 The alkyl group of the "alkyl group which may have a substituent" which can constitute R is not particularly limited, and examples thereof include alkyl groups having 1 to 5 carbon atoms. 13 The alkyl group that can constitute R is preferably a methyl group or an ethyl group. The substituent is not particularly limited, and examples thereof include halogen atoms such as chlorine atom, fluorine atom, bromine atom, and iodine atom. 13When the alkyl group that can constitute the above is substituted with a halogen atom, some or all of the hydrogen atoms in the alkyl group may be substituted with the above halogen atoms.

[0059] R in formula (III) and formula (c) 14 The halogen atom that can constitute the group is not particularly limited, and examples thereof include a chlorine atom, a fluorine atom, a bromine atom, an iodine atom, etc. Among these, a fluorine atom is preferred.

[0060] Furthermore, R in formula (III) and formula (c) 14 Examples of organic groups that can constitute R include unsubstituted alkyl groups, alkyl groups substituted with halogen atoms, alkoxy groups, and alkoxy groups substituted with halogen atoms. 14 The unsubstituted alkyl group that can constitute R is not particularly limited, and examples thereof include unsubstituted alkyl groups having 1 to 5 carbon atoms. Among these, a methyl group or an ethyl group is preferred. 14 The alkyl group substituted with a halogen atom that can constitute R is not particularly limited, and examples thereof include groups having a structure in which some or all of the hydrogen atoms in the alkyl group have been substituted with the above-mentioned halogen atoms. 14 The alkoxy group that can constitute R is not particularly limited, and examples thereof include alkoxy groups having 1 to 5 carbon atoms. Among these, a methoxy group or an ethoxy group is preferred. 14 The alkoxy group substituted with a halogen atom that can constitute the above group is not particularly limited, and examples thereof include groups having a structure in which some or all of the hydrogen atoms in the alkoxy group have been substituted with the above halogen atoms.

[0061] In addition, R 14 When there are a plurality of R (i.e., when p is an integer of 2 or more and 5 or less), 14 may be the same or different from each other.

[0062] The monomer (c) represented by formula (c) is not particularly limited, and examples thereof include α-methylstyrene (AMS) and its derivatives, such as the following monomers (c-1) to (c-14).

[0063] From the viewpoint of improving the ease of preparation of the copolymer, the monomer unit (III) preferably does not have a fluorine atom, and is more preferably a structural unit derived from α-methylstyrene. 11 and R 12 is a hydrogen atom, and R 13 It is preferred that is a methyl group and p=0.

[0064] The proportion of the monomer unit (III) in the copolymer is not particularly limited, and is preferably 20 mol% or more, more preferably 30 mol% or more, and even more preferably 40 mol% or more, and is preferably 80 mol% or less, preferably 75 mol% or less, and more preferably 70 mol% or less, when the total amount of all monomer units in the copolymer is 100 mol%.

[0065] <Properties of the Copolymer> [Weight-Average Molecular Weight (Mw)] The weight-average molecular weight (Mw) of the copolymer is preferably 20,000 or more, more preferably 50,000 or more, even more preferably 300,000 or more, and preferably 500,000 or less, more preferably 400,000 or less, and even more preferably 350,000 or less. If the weight-average molecular weight (Mw) of the copolymer is equal to or greater than the above-mentioned lower limit, excessive increase in the solubility of the resist film in the developer can be suppressed even at a low irradiation dose, and a resist pattern with a better shape can be formed. On the other hand, if the weight-average molecular weight (Mw) of the copolymer is equal to or less than the above-mentioned upper limit, a positive resist composition can be easily prepared. In this specification, the "weight-average molecular weight" can be measured by the method described in the Examples.

[0066] [Number Average Molecular Weight (Mn)] The number average molecular weight (Mn) of the copolymer is preferably 7,000 or more, more preferably 10,000 or more, even more preferably 20,000 or more, and preferably 200,000 or less, more preferably 150,000 or less, even more preferably 140,000 or less, and even more preferably 100,000 or less. If the number average molecular weight of the copolymer is equal to or greater than the above-mentioned lower limit, excessive increase in the solubility of the resist film in the developer at a low irradiation dose can be further suppressed, and a resist pattern with a better shape can be formed. On the other hand, if the number average molecular weight of the copolymer is equal to or less than the above-mentioned upper limit, a positive resist composition can be more easily prepared. In this specification, the "number average molecular weight" can be measured by the method described in the Examples.

[0067] [Molecular Weight Distribution (Mw / Mn)] The molecular weight distribution (Mw / Mn) of the copolymer is preferably 1.10 or more, more preferably 1.20 or more, even more preferably 1.50 or more, and preferably 3.00 or less, more preferably 2.70 or less, and even more preferably 2.50 or less. If the molecular weight distribution (Mw / Mn) of the copolymer is equal to or greater than the lower limit, the ease of production of the copolymer can be improved. On the other hand, if the molecular weight distribution (Mw / Mn) of the copolymer is equal to or less than the upper limit, the shape of the obtained resist pattern can be further improved. In this specification, the "molecular weight distribution" can be determined by calculating the ratio of the weight average molecular weight to the number average molecular weight (weight average molecular weight / number average molecular weight).

[0068] <Method for Preparing Copolymer> The method for preparing the copolymer is not particularly limited. For example, a copolymer containing monomer unit (I), monomer unit (II), and monomer unit (III) can be prepared by polymerizing a monomer composition containing monomer (a), monomer (b), monomer (c), and any monomer copolymerizable with these monomers, recovering the resulting copolymer, and optionally purifying it. The composition, molecular weight distribution, number average molecular weight, and weight average molecular weight of the copolymer can be adjusted by changing the polymerization conditions and purification conditions. Specifically, for example, the number average molecular weight and weight average molecular weight can be increased by lowering the polymerization temperature. The number average molecular weight and weight average molecular weight can be increased by shortening the polymerization time. Furthermore, purification can narrow the molecular weight distribution.

[0069] [Polymerization of Monomer Composition] The monomer composition used to prepare the copolymer may be, for example, a mixture of monomer components including monomer (a), monomer (b), monomer (c), and any monomer copolymerizable with these monomers, an optionally usable solvent, an optionally usable polymerization initiator, and any additives. Polymerization of the monomer composition can be carried out using known methods. Among these, cyclopentanone, water, or the like is preferably used as the solvent. Furthermore, azobisisobutyronitrile, dimethyl 2,2'-azobis(2-methylpropionate), or the like is preferably used as the polymerization initiator.

[0070] The polymer obtained by polymerizing the monomer composition can be recovered by adding a good solvent such as tetrahydrofuran to a solution containing the polymer, and then dropping the solution to which the good solvent has been added into a poor solvent such as methanol, ethanol, 1-propanol, 1-butanol, 1-pentanol, or hexane to coagulate the polymer, without any particular limitation.

[0071] [Purification of Polymer] The purification method used to purify the obtained polymer is not particularly limited, and known purification methods such as reprecipitation and column chromatography can be used. Among them, the reprecipitation method is preferred as the purification method. The purification of the polymer may be repeated multiple times.

[0072] Purification of a polymer by the reprecipitation method is preferably carried out, for example, by dissolving the obtained polymer in a good solvent such as tetrahydrofuran, and then dropping the resulting solution into a mixed solvent of a good solvent such as tetrahydrofuran and a poor solvent such as methanol, ethanol, 1-propanol, 1-butanol, 1-pentanol, or hexane to precipitate a portion of the polymer. In this way, by dropping a solution of the polymer into a mixed solvent of a good solvent and a poor solvent to perform purification, the molecular weight distribution, number average molecular weight, and weight average molecular weight of the resulting copolymer can be easily adjusted by changing the type and mixing ratio of the good solvent and poor solvent. Specifically, for example, the molecular weight of the copolymer precipitated in the mixed solvent can be increased by increasing the proportion of the good solvent in the mixed solvent.

[0073] When purifying a polymer by the reprecipitation method, a polymer precipitated in a mixed solvent of a good solvent and a poor solvent may be used as the copolymer, as long as the copolymer has the desired properties. Alternatively, a polymer not precipitated in the mixed solvent (i.e., a polymer dissolved in the mixed solvent) may be used. Here, the polymer not precipitated in the mixed solvent can be recovered from the mixed solvent by a known method such as concentration to dryness.

[0074] (Positive Resist Composition) The positive resist composition of the present invention comprises the copolymer of the present invention and a solvent. Because the positive resist composition of the present invention contains the above-mentioned copolymer of the present invention, it is possible to form a resist pattern with a good shape while increasing the exposure margin of the resulting resist.

[0075] <Copolymer> As the copolymer, the copolymer of the present invention described above can be used.

[0076] When the total of all components of the positive resist composition is taken as 100 mass %, the content of the copolymer in the positive resist composition is preferably 0.5 mass % or more, more preferably 1 mass % or more, and even more preferably 1.5 mass % or more, and is preferably 15 mass % or less, more preferably 10 mass % or less, and even more preferably 5 mass % or less.

[0077] <Solvent> There are no particular restrictions on the solvent, as long as it is capable of dissolving the copolymer of the present invention, and it is possible to use known solvents such as those described in Japanese Patent No. 5938536. Among these, from the perspective of obtaining a positive resist composition with an appropriate viscosity and improving the coatability of the positive resist composition, it is preferable to use anisole, propylene glycol monomethyl ether acetate (PGMEA), cyclopentanone, cyclohexanone, or isoamyl acetate as the solvent, and it is more preferable to use isoamyl acetate.

[0078] <Other Components> In addition to the components described above, the positive resist composition of the present invention may optionally further contain known additives that can be incorporated into resist compositions. There are no particular restrictions on the amount of additives that can be incorporated, and an appropriate amount can be added depending on the application.

[0079] <Preparation of Positive Resist Composition> The positive resist composition can be prepared by mixing the copolymer of the present invention, a solvent, and any known additives that can be used. There are no particular limitations on the mixing method, and mixing can be carried out using a known method. Alternatively, the resist composition can be prepared by mixing the components and then filtering the mixture.

[0080] [Filtration] The method for filtering the mixture is not particularly limited, and for example, it can be performed using a filter. The filter is not particularly limited, and examples include fluorocarbon, cellulose, nylon, polyester, and hydrocarbon-based filter membranes. Among these, from the viewpoint of effectively preventing impurities such as metals from being mixed into the positive resist composition from metal piping, etc., which may be used during the preparation of the copolymer of the present invention, preferred materials for the filter include polyfluorocarbons such as polyethylene, polypropylene, polytetrafluoroethylene, and Teflon (registered trademark), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymers (PFA), nylon, and composite membranes of polyethylene and nylon. Filters such as those disclosed in U.S. Pat. No. 6,103,122 may be used. Alternatively, commercially available filters such as Zeta Plus (registered trademark) 40Q manufactured by CUNO Incorporated may be used. Furthermore, the filter may contain a strong or weak cationic ion exchange resin. The average particle size of the ion exchange resin is not particularly limited, but is preferably 2 μm or more and 10 μm or less. Examples of cation exchange resins include sulfonated phenol-formaldehyde condensates, sulfonated phenol-benzaldehyde condensates, sulfonated styrene-divinylbenzene copolymers, sulfonated methacrylic acid-divinylbenzene copolymers, and other types of polymers containing sulfonic or carboxylic acid groups. + Counterion, NH 4 + counter ions or alkali metal counter ions, e.g., K + and Na + Counterions are provided. The cation exchange resin preferably has hydrogen counterions. Examples of such cation exchange resins include H +Sulfonated styrene-divinylbenzene copolymers with counterions, such as Microlite® PrCH from Purolite Corp. Such cation exchange resins are commercially available as AMBERLYST® from Rohm and Haas.

[0081] The pore size of the filter is preferably from 0.001 μm to 1 μm, inclusive. If the pore size of the filter is within this range, it is possible to sufficiently prevent impurities such as metals from being mixed into the positive resist composition.

[0082] (Method of Forming Resist Pattern) The method of forming a resist pattern of the present invention includes at least the steps of forming a resist film using the above-described positive resist composition of the present invention (resist film formation step), exposing the resist film (exposure step), and developing the exposed resist film (development step). Furthermore, the method of forming a resist pattern of the present invention may also include, for example, a step of forming an underlayer film on the substrate on which the resist film will be formed (underlayer film formation step) prior to the resist film formation step. The method of forming a resist pattern of the present invention may also include a step of heating the resist film between the exposure step and the development step (post-exposure bake (PEB) step), and / or a step of removing the developer after the development step (developer removal step). After forming a resist pattern by the method of forming a resist pattern, the method of forming a resist pattern of the present invention may also include a step of etching the underlayer film and / or the substrate (etching step). Because the method of forming a resist pattern of the present invention uses the positive resist composition of the present invention as the positive resist composition, a resist pattern with a good shape can be formed with a wide exposure margin.

[0083] <Underlayer Film Formation Step> In the underlayer film formation step, which can be optionally performed before the resist film formation step, an underlayer film is formed on a substrate. By providing the underlayer film on the substrate, the surface of the substrate is made hydrophobic. This increases the affinity between the substrate and the resist film, thereby improving the adhesion between the substrate and the resist film. The underlayer film may be an inorganic underlayer film or an organic underlayer film.

[0084] The inorganic underlayer film can be formed by applying an inorganic material onto a substrate and then baking it, etc. Examples of inorganic materials include silicon-based materials.

[0085] The organic underlayer film can be formed by applying an organic material to a substrate to form a coating film and drying it. The organic material is not limited to those sensitive to light or electron beams, and can include, for example, resist materials and resin materials commonly used in the semiconductor and liquid crystal fields. Among these, the organic material is preferably a material capable of forming an organic underlayer film that can be etched, particularly dry etched. With such an organic material, the organic underlayer film can be etched using a pattern formed by processing a resist film, thereby transferring the pattern to the underlayer film and forming a pattern in the underlayer film. Among these, the organic material is preferably a material capable of forming an organic underlayer film that can be etched by oxygen plasma etching or the like. Examples of organic materials used to form the organic underlayer film include AL412 from Brewer Science.

[0086] The organic material can be applied by a conventional method using spin coating or a spinner. The method for drying the coating film can be any method capable of volatilizing the solvent contained in the organic material, such as baking. The baking conditions are not particularly limited, but the baking temperature is preferably 80°C or higher and 300°C or lower, and more preferably 200°C or higher and 300°C or lower. The baking time is preferably 30 seconds or longer, more preferably 60 seconds or longer, and preferably 500 seconds or shorter, more preferably 400 seconds or shorter, even more preferably 300 seconds or shorter, and particularly preferably 180 seconds or shorter. The thickness of the underlayer film after drying the coating film is not particularly limited, but is preferably 10 nm or higher and 100 nm or lower.

[0087] [Substrate] Here, the substrate on which the underlayer film or resist film can be formed in the resist pattern forming method is not particularly limited, and examples that can be used include a substrate having an insulating layer and copper foil provided on the insulating layer, which is used in the manufacture of printed circuit boards, etc.; and a mask blank having a light-shielding layer formed on a substrate.

[0088] The substrate material may be, for example, metal (silicon, copper, chromium, iron, aluminum, etc.), glass, titanium oxide, silicon dioxide (SiO 2 Examples of suitable substrates include inorganic materials such as silica and mica; nitrides such as SiN; oxynitrides such as SiON; and organic materials such as acrylic, polystyrene, cellulose, cellulose acetate, and phenolic resin. Among these, metals are preferred as the substrate material. By using, for example, a silicon substrate, a silicon dioxide substrate, or a copper substrate, preferably a silicon substrate or a silicon dioxide substrate, as the substrate, a cylindrical structure can be formed.

[0089] The size and shape of the substrate are not particularly limited. The surface of the substrate may be smooth, curved, or uneven, and may be a thin plate-shaped substrate.

[0090] The surface of the substrate may be subjected to a surface treatment as necessary. For example, in the case of a substrate having hydroxyl groups on its surface layer, the surface of the substrate can be treated using a silane coupling agent capable of reacting with the hydroxyl groups. This changes the surface layer of the substrate from hydrophilic to hydrophobic, thereby improving the adhesion between the substrate and the underlayer film or between the substrate and the resist layer. In this case, the silane coupling agent is not particularly limited, but hexamethyldisilazane is preferred.

[0091] <Resist film forming step> In the resist film forming step, the positive resist composition of the present invention is applied onto a workpiece such as a substrate to be processed using the resist pattern (or onto an underlayer film if an underlayer film has been formed) to obtain a coating layer (coating step), and then the solvent is removed from the obtained coating layer to form a resist film (drying step).

[0092] [Coating Step] The workpiece to be coated with the positive resist composition of the present invention in the coating step is not particularly limited, and examples that can be used include semiconductor substrates used in the manufacture of semiconductor devices, etc.; substrates having an insulating layer and copper foil provided on the insulating layer, used in the manufacture of printed circuit boards, etc.; and mask blanks having a light-shielding layer formed on a substrate. Furthermore, there are no particular limitations on the method for coating the positive resist composition of the present invention, and any known method can be used.

[0093] [Drying Step] The method for removing the solvent from the coating layer is not particularly limited, and a drying method commonly used in forming a resist film can be used. However, it is preferable to form a resist film by heating (prebaking) the positive resist composition. Here, the temperature at which the coating layer is dried (drying temperature) is preferably 100°C or higher, more preferably 110°C or higher, from the viewpoint of adhesion between the resist film formed through the drying step and the workpiece. Furthermore, from the viewpoint of reducing the thermal influence on the workpiece and the resist film, it is preferably 250°C or lower, more preferably 200°C or lower. The time for drying the coating layer (drying time) is preferably more than 10 seconds, more preferably 30 seconds or higher, even more preferably 1 minute or higher, from the viewpoint of sufficiently improving adhesion between the resist film formed by performing the drying step at a lower temperature range and the workpiece. From the viewpoint of reducing the change in molecular weight of the polymer in the resist film before and after the drying step, it is preferably 60 minutes or lower, more preferably 30 minutes or lower.

[0094] <Exposure Step> In the exposure step, the resist film formed in the resist film formation step is irradiated with ionizing radiation or the like to write a desired pattern. For electron beam irradiation, known writing devices such as electron beam writing devices and EUV exposure devices can be used. Here, ionizing radiation is radiation that has sufficient energy to ionize atoms or molecules. In contrast, non-ionizing radiation is radiation that does not have sufficient energy to ionize atoms or molecules.

[0095] Examples of ionizing radiation include electron beams, extreme ultraviolet rays, gamma rays, X-rays, alpha rays, heavy particle beams, proton beams, beta rays, and ion beams. Among these, electron beams or extreme ultraviolet rays are preferred as ionizing radiation, and electron beams are more preferred. The wavelength of extreme ultraviolet rays is not particularly limited, and can be, for example, 1 nm or more and 30 nm or less, and preferably 13.5 nm.

[0096] The nonionizing radiation is not particularly limited, but it is preferable to use nonionizing radiation having a wavelength of 300 nm or less. Examples of nonionizing radiation having a wavelength of 300 nm or less include far ultraviolet radiation excluding extreme ultraviolet radiation (wavelength: 40 nm or more and 200 nm or less) and near ultraviolet radiation (wavelength: more than 200 nm and 300 nm or less). Among these, KrF excimer laser radiation (wavelength: 248 nm) and ArF excimer laser radiation (wavelength: 193 nm) are preferred.

[0097] <Post-exposure bake step> In the post-exposure bake step, which may be optionally performed, the resist film exposed in the exposure step is heated. By performing the post-exposure bake step, the surface roughness of the resist pattern can be reduced.

[0098] Here, the heating temperature is preferably 70° C. or higher, more preferably 80° C. or higher, and even more preferably 90° C. or higher, and is preferably 200° C. or lower, more preferably 170° C. or lower, and even more preferably 150° C. or lower. When the heating temperature is within the above range, the clarity of the resist pattern can be improved while the surface roughness of the resist pattern can be effectively reduced.

[0099] The time for heating the resist film in the post-exposure bake step (heating time) is preferably 10 seconds or longer, more preferably 20 seconds or longer, and even more preferably 30 seconds or longer. A heating time of 10 seconds or longer can further improve the clarity of the resist pattern while sufficiently reducing the surface roughness of the resist pattern. On the other hand, from the viewpoint of production efficiency, the heating time is, for example, preferably 10 minutes or shorter, more preferably 5 minutes or shorter, and even more preferably 3 minutes or shorter.

[0100] The method for heating the resist film in the post-exposure bake step is not particularly limited, and examples thereof include a method of heating the resist film on a hot plate, a method of heating the resist film in an oven, and a method of blowing hot air onto the resist film.

[0101] <Developing Step> In the developing step, the exposed resist film (or the exposed and heated resist film if a post-exposure bake step has been performed) is developed to form a developed film on the workpiece. Here, the resist film can be developed, for example, by contacting the resist film with a developer. The method for contacting the resist film with the developer is not particularly limited, and known methods such as immersing the resist film in the developer or applying the developer to the resist film can be used.

[0102] [Developer] The developer can be appropriately selected depending on the properties of the copolymer of the present invention. Specifically, when selecting a developer, it is preferable to select a developer that does not dissolve the resist film before the exposure step, but can dissolve the exposed portion of the resist film after the exposure step. One type of developer may be used alone, or two or more types may be mixed in any ratio. As the developer, for example, 1,1,1,2,3,4,4,5,5,5-decafluoropentane (CF 3 CFHCFHCF 2 CF 3 ), 1,1,1,2,2,3,3,4,4,5,5,6,6-tridecafluorohexane, 1,1,1,2,2,3,4,5,5,5-decafluoropentane, 1,1,1,3,3-pentafluorobutane, 1,1,1,2,2,3,3,4,4-nonafluorohexane, and other hydrofluorocarbons; 2,2-dichloro-1,1,1-trifluoroethane, 1,1-dichloro-1-fluoroethane, 1,1-dichloro-2,2,3,3,3-pentafluoropropane (CF 3 CF 2 CHCl 2 ), 1,3-dichloro-1,1,2,2,3-pentafluoropropane (CClF 2 CF 2CHClF), methyl nonafluorobutyl ether (CF 3 CF 2 CF 2 CF 2 OCH 3 ), methyl nonafluoroisobutyl ether, ethyl nonafluorobutyl ether (CF 3 CF 2 CF 2 CF 2 O.C. 2 H 5 ), ethyl nonafluoroisobutyl ether, perfluorohexyl methyl ether (CF 3 CF 2 CF (OCH 3 ) C 3 F 7 ) and hydrofluoroethers such as CF 4 , C 2 F 6 , C 3 F 8 , C 4 F 8 , C 4 F 10 , C 5 F 12 , C 6 F 12 , C 6 F 14 , C 7 F 14 , C 7 F 16 , C 8 F 18 , C 9 F 20Examples of suitable developers that can be used include perfluorocarbons such as fluorine-based solvents, perfluorocarbons such as ethanol, 1-propanol, 2-propanol (isopropyl alcohol), 1-butanol, 2-butanol, 1-pentanol, 2-pentanol, and 3-pentanol; alkyl acetate solvents such as amyl acetate and hexyl acetate; mixtures of fluorine-based solvents and alcohol-based solvents; mixtures of fluorine-based solvents and alkyl acetate solvents; mixtures of alcohol-based solvents and alkyl acetate solvents; and mixtures of fluorine-based solvents, alcohol-based solvents, and alkyl acetate solvents. Among these, from the viewpoint of imparting a better shape to the resist pattern, it is preferable to use an alcohol-based solvent as the developer, and it is more preferable to use isopropyl alcohol.

[0103] <Developer Removal Step> In the developer removal step optionally included in the resist pattern formation method, the developer is removed from the developed resist film to form a resist pattern on the workpiece. The developer can be removed by air blowing using a gas such as nitrogen, or by rinsing using a rinse solution. Here, the method for contacting the developed resist film with the rinse solution in the rinse process is not particularly limited, and known methods such as immersing the resist film in the rinse solution or applying the rinse solution to the resist film can be used. Specific examples of rinse solutions include the same developers as those exemplified in the "Development Step" section, as well as hydrocarbon solvents such as octane and heptane, and water. Here, the rinse solution may contain a surfactant. When selecting a rinse solution, it is preferable to select a rinse solution that is less likely to dissolve the resist film before the exposure step than the developer used in the development step and that is easily mixed with the developer.

[0104] <Etching Step> In the etching step, which can be optionally performed, the underlayer film and / or the substrate are etched using the above-mentioned resist pattern as a mask to form a pattern on the underlayer film and / or the substrate. In this case, the number of etchings is not particularly limited, and may be one or more times. Furthermore, the etching may be dry etching or wet etching, but dry etching is preferred. Dry etching can be performed using a known dry etching device. The etching gas used in dry etching can be appropriately selected depending on the elemental composition of the underlayer film and the substrate to be etched, etc. Examples of the etching gas include CHF 3 , C.F. 4 , C 2 F 6 , C 3 F 8 , SF 6 fluorine-based gases such as Cl 2 , BCl 3 Chlorine-based gases such as O 2 , O 3 , H 2 Oxygen-based gases such as O; 2 , N.H. 3 , CO, CO 2 , C.H. 4 , C 2 H 2 , C 2 H 4 , C 2 H6, C 3 H 4 , C 3 H 6 , C 3 H 8 , HF, HI, HBr, HCl, NO, BCl 3 reducing gases such as He, N 2 , and inert gases such as Ar. These gases may be used alone or in combination of two or more. For dry etching of an inorganic underlayer film, an oxygen-based gas is usually used. For dry etching of a substrate, a fluorine-based gas is usually used, and a mixture of a fluorine-based gas and an inert gas is preferably used.

[0105] Furthermore, if necessary, the underlayer film remaining on the substrate may be removed before or after etching the substrate. When the underlayer film is removed before etching the substrate, the underlayer film may be a patterned or unpatterned underlayer film.

[0106] Here, examples of methods for removing the underlayer film include the above-mentioned dry etching. In the case of an inorganic underlayer film, the underlayer film may be removed by contacting the underlayer film with a liquid such as a basic or acidic liquid, preferably a basic liquid. The basic liquid is not particularly limited, and examples thereof include alkaline hydrogen peroxide. The method for removing the underlayer film by wet stripping using alkaline hydrogen peroxide is not particularly limited as long as it allows the underlayer film and alkaline hydrogen peroxide to come into contact with each other for a certain period of time under heated conditions. Examples include a method of immersing the underlayer film in heated alkaline hydrogen peroxide, a method of spraying alkaline hydrogen peroxide onto the underlayer film in a heated environment, and a method of coating the underlayer film with heated alkaline hydrogen peroxide. After performing any of these methods, the substrate is washed with water and dried to obtain a substrate from which the underlayer film has been removed.

[0107] Below, an example of a method for forming a resist pattern using the positive resist composition of the present invention and a method for etching an underlayer film and a substrate using the formed resist pattern will be described. However, since the substrate used in the following example and the conditions in each step can be the same as the substrate and conditions in each step described above, explanations will be omitted below. It should be noted that the method for forming a resist pattern is not limited to the method shown in the following example.

[0108] An example of the resist pattern forming method is a resist pattern forming method using an electron beam or EUV, which includes the above-mentioned underlayer film forming step, resist film forming step, exposure step, developing step, and developer removing step.An example of the etching method is a method in which the resist pattern formed by the resist pattern forming method is used as a mask, and includes an etching step.

[0109] Specifically, in the underlayer film formation step, an inorganic material is applied to a substrate and baked to form an inorganic underlayer film. Next, in the resist film formation step, a positive resist composition of the present invention is applied to the inorganic underlayer film formed in the underlayer film formation step, and the composition is dried to form a resist film. Then, in the exposure step, the resist film formed in the resist film formation step is irradiated with EUV light to write a desired pattern. Furthermore, in the development step, the resist film exposed in the exposure step is brought into contact with a developer to develop the resist film, thereby forming a resist pattern on the underlayer film. Then, in the developer removal step, the resist film developed in the development step is brought into contact with a rinse solution to rinse the developed resist film. Then, in the etching step, the underlayer film is etched using the resist pattern as a mask to form a pattern in the underlayer film. Next, the substrate is etched using the patterned underlayer film as a mask to form a pattern on the substrate.

[0110] The present invention will be specifically explained below based on examples, but the present invention is not limited to these examples. Furthermore, in a copolymer produced by copolymerizing a plurality of types of monomers, the proportion of a monomer unit formed by polymerizing a certain monomer in the copolymer usually coincides with the ratio (feed ratio) of the certain monomer to all the monomers used in the polymerization of the copolymer, unless otherwise specified. In the examples and comparative examples, the proportion of the monomer units in the copolymer, the number average molecular weight, weight average molecular weight and molecular weight distribution of the copolymer were measured or calculated by the following methods. In the examples and comparative examples, the exposure margin of the resist and the shape of the resist pattern were evaluated by the following methods. <Proportion of Monomer Units in Copolymer> For the copolymers obtained in the examples and comparative examples, 13The proportion of each monomer unit in the copolymer was calculated using C-NMR. Specifically, the copolymers obtained in the Examples and Comparative Examples were dissolved in chloroform-d, 99.8% (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) to a concentration of 10% by mass, and the proportion of each monomer unit in the copolymer was calculated using this solution with a nuclear magnetic resonance spectrometer (manufactured by JEOL Ltd., 500 MHz). <Number Average Molecular Weight, Weight Average Molecular Weight, and Molecular Weight Distribution> The number average molecular weight (Mn) and weight average molecular weight (Mw) of the copolymers obtained in the Examples and Comparative Examples were measured using gel permeation chromatography, and the molecular weight distribution (Mw / Mn) was calculated. Specifically, using a gel permeation chromatograph (manufactured by Tosoh Corporation, HLC-8420) and tetrahydrofuran as the developing solvent, the number average molecular weight (Mn) and weight average molecular weight (Mw) of the copolymer were determined in terms of standard polystyrene. The molecular weight distribution (Mw / Mn) was then calculated. <Exposure Margin> Resist patterns were formed using the positive resist compositions obtained in the examples and comparative examples, and the exposure margin was evaluated. Specifically, first, a spin coater (MS-A150, manufactured by Mikasa) was used to apply the positive resist composition to a thickness of 50 nm on a silicon wafer with a diameter of 4 inches. Next, the applied positive resist composition was heated on a hot plate at a temperature of 170°C for 1 minute to form a resist film on the silicon wafer (resist film formation step). The resist film had a thickness of 50 nm. Then, an electron beam lithography system (ELS-S50, manufactured by Elionix) was used to coat the resist film at 100 μC / cm 2 to 400 μC / cm 2 Within the range of 10 μC / cm 2The resist film was exposed to light at different exposure doses, and a pattern was written (exposure step). After the exposure step, the resist film was developed for 1 minute at 23°C using isopropyl alcohol (IPA) as the developer (development step). The developer was then removed by nitrogen blowing to form a resist pattern (developer removal step). The formed resist pattern was then observed for pattern separation and pattern collapse. The lines (unexposed areas) and spaces (exposed areas) of the resist pattern were each 30 nm. The exposure margin was evaluated according to the following criteria. The results are shown in Table 1. A: The difference between the exposure dose at which pattern separation begins and the exposure dose at which pattern collapse occurs is 50 μC / cm 2 B: The difference between the exposure dose at which pattern separation begins and the exposure dose at which pattern collapse occurs is 10 μC / cm 2 More than 50μC / cm 2 C: The difference between the exposure dose at which pattern separation begins and the exposure dose at which pattern collapse occurs is less than 10 μC / cm 2 <Resist Pattern Shape> Resist patterns were formed using the positive resist compositions obtained in the Examples and Comparative Examples, and the resist pattern shapes were evaluated. Specifically, the shapes of patterns exposed at the median exposure dose within the range from pattern separation to pattern collapse when the exposure margin was evaluated above were observed using a scanning electron microscope. The shapes of the resist patterns were then evaluated according to the following criteria. The results are shown in Table 1. A: The sidewall shape of the resist pattern is smooth. B: The sidewall shape of the resist pattern is rough.

[0111] Example 1 Preparation of Copolymer A1 A monomer composition A1 containing 5.98 g of 1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl α-chloroacrylate (ACAFPh) as the monomer (a), 0.48 g of 2-adamantyl α-chloroacrylate (ACA2Ad) as the monomer (b), 3.54 g of α-methylstyrene (AMS) as the monomer (c), 0.00013 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as a polymerization initiator, and 6.66 g of cyclopentanone as a solvent was placed in a glass container, the glass container was sealed and purged with nitrogen, and the mixture was stirred in a constant temperature bath at 78° C. under a nitrogen atmosphere for 6 hours. After that, the temperature was returned to room temperature, and the glass container was opened to the atmosphere. Then, 16.69 g of THF (tetrahydrofuran) was added to the obtained solution. Then, the solution to which THF had been added was dropped into 400 g of methanol as a solvent to precipitate a polymer. Thereafter, the solution containing the precipitated polymer was filtered using a Kiriyama funnel to obtain a white coagulated product (copolymer A1). The proportion of the monomer units in the obtained copolymer A1 was 13 Calculations using C-NMR revealed that copolymer A1 was a polymer containing 47.2 mol% of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I), 3.4 mol% of α-chloroacrylate-2-adamantyl units as monomer units (II), and 49.4 mol% of α-methylstyrene units as monomer units (III). Thereafter, the number average molecular weight, weight average molecular weight, and molecular weight distribution of the obtained copolymer A1 were measured. The results are shown in Table 1.

[0112] <Preparation of Positive Resist Composition> The copolymer A1 prepared as described above was dissolved in isoamyl acetate as a solvent to prepare a positive resist composition with a concentration of 2 mass%. A resist pattern was formed using the obtained positive resist composition, and the exposure margin and shape of the resist pattern were evaluated. The results are shown in Table 1.

[0113] Example 2 Various operations, measurements and evaluations were carried out in the same manner as in Example 1, except that in the preparation of a copolymer, instead of the monomer composition A1, a monomer composition A2 containing 5.98 g of 1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl α-chloroacrylate (ACAFPh) as the monomer (a), 0.48 g of α-chloroacrylic acid-norbornane lactone (ACANBL) as the monomer (b), 3.54 g of α-methylstyrene (AMS) as the monomer (c), 0.00017 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as the polymerization initiator, and 6.62 g of cyclopentanone as the solvent was prepared. The results are shown in Table 1. The obtained copolymer A2 was a copolymer containing 45.1 mol % of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I), 4.2 mol % of α-chloroacrylic acid-norbornane lactone units as monomer units (II), and 50.7 mol % of α-methylstyrene units as monomer units (III).

[0114] Example 3 Various operations, measurements and evaluations were carried out in the same manner as in Example 1, except that in the preparation of a copolymer, instead of the monomer composition A1, a monomer composition A3 containing 6.13 g of 1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl α-chloroacrylate (ACAFPh) as the monomer (a), 0.25 g of methyl α-chloroacrylate (ACAM) as the monomer (b), 3.63 g of α-methylstyrene (AMS) as the monomer (c), 0.0024 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as the polymerization initiator, and 6.42 g of cyclopentanone as the solvent was prepared. The results are shown in Table 1. The obtained copolymer A3 was a copolymer containing 47.4 mol % of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I), 2.8 mol % of α-chloroacrylate methyl units as monomer units (II), and 49.8 mol % of α-methylstyrene units as monomer units (III).

[0115] Example 4 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that copolymer A4 prepared as follows was used instead of copolymer A1. The results are shown in Table 1. [Preparation of Polymer] A monomer composition A4 containing 10.23 g of 1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl α-chloroacrylate (ACAFPh) as the monomer (a), 0.82 g of 2-adamantyl α-chloroacrylate (ACA2Ad) as the monomer (b), 6.04 g of α-methylstyrene (AMS) as the monomer (c), and 0.174 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as a polymerization initiator was placed in a glass container. Further, 55.48 g of an aqueous sodium laurate solution with a solids content of 7.5% was added, and the glass container was sealed and purged with nitrogen, and the mixture was stirred in a constant temperature bath at 75° C. under a nitrogen atmosphere for 3 hours. Thereafter, the temperature was returned to room temperature, and the glass container was opened to the atmosphere. The obtained solution was then added dropwise to 569.21 g of methanol to precipitate a polymer. The precipitated polymer was then recovered by filtration. [Polymer purification] The polymer recovered by filtration was dissolved in 41.02 g of THF, and a mixed solution of 187.14 g of THF and 325.57 g of methanol was added dropwise to the obtained solution to precipitate a white coagulate (polymer). Thereafter, the polymer recovered by decantation was dissolved in 27.34 g of THF, and the obtained solution was added dropwise to 273.44 g of methanol to precipitate a polymer. Thereafter, the solution containing the precipitated polymer was filtered using a Kiriyama funnel to obtain a coagulate (copolymer A4). The ratio of the monomer units in the obtained polymer A4 was 13 Calculation using a C-NMR method revealed that polymer A4 was a copolymer containing 47.1 mol % of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I), 5.5 mol % of α-chloroacrylate-2-adamantyl units as monomer units (II), and 47.4 mol % of α-methylstyrene units as monomer units (III).

[0116] Example 5 Various operations, measurements and evaluations were carried out in the same manner as in Example 4, except that in the preparation of a copolymer, instead of the monomer composition A4, a monomer composition A5 containing 10.21 g of 1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl α-chloroacrylate (ACAFPh) as the monomer (a), 0.83 g of α-chloroacrylic acid-norbornane lactone (ACANBL) as the monomer (b), 6.04 g of α-methylstyrene (AMS) as the monomer (c), and 0.168 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as a polymerization initiator was prepared. The results are shown in Table 1. The obtained polymer A5 was a polymer containing 51.7 mol % of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I), 2.5 mol % of α-chloroacrylic acid-norbornane lactone units as monomer units (II), and 45.8 mol % of α-methylstyrene units as monomer units (III).

[0117] Example 6 Various operations, measurements and evaluations were carried out in the same manner as in Example 4, except that in the preparation of a copolymer, instead of the monomer composition A4, a monomer composition A6 containing 10.20 g of 1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl α-chloroacrylate (ACAFPh) as the monomer (a), 0.41 g of methyl α-chloroacrylate (ACAM) as the monomer (b), 6.04 g of α-methylstyrene (AMS) as the monomer (c), and 0.190 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as a polymerization initiator was prepared. The results are shown in Table 1. The obtained copolymer A6 was a polymer containing 50.8 mol % of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I), 2.9 mol % of α-chloroacrylate methyl units as monomer units (II), and 46.3 mol % of α-methylstyrene units as monomer units (III).

[0118] Example 7 Various operations, measurements and evaluations were carried out in the same manner as in Example 1, except that in the preparation of a copolymer, instead of the monomer composition A1, a monomer composition A7 containing 3.25 g of 1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl α-chloroacrylate (ACAFPh) as the monomer (a), 0.59 g of 2-adamantyl α-chloroacrylate (ACA2Ad) as the monomer (b), 2.16 g of α-methylstyrene (AMS) as the monomer (c), 0.00011 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as the polymerization initiator, and 3.97 g of cyclopentanone as the solvent was prepared. The results are shown in Table 1. The obtained copolymer A7 was a polymer containing 46.9 mol % of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I), 4.4 mol % of α-chloroacrylate-2-adamantyl units as monomer units (II), and 48.7 mol % of α-methylstyrene units as monomer units (III).

[0119] Example 8 Various operations, measurements and evaluations were carried out in the same manner as in Example 1, except that in the preparation of a polymer, instead of the monomer composition A1, a monomer composition A8 containing 3.25 g of 1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl α-chloroacrylate (ACAFPh) as the monomer (a), 0.59 g of α-chloroacrylic acid-norbornane lactone (ACANBL) as the monomer (b), 2.16 g of α-methylstyrene (AMS) as the monomer (c), 0.00011 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as the polymerization initiator, and 3.97 g of cyclopentanone as the solvent was prepared. The results are shown in Table 1. The obtained copolymer A8 was a polymer containing 47.3 mol % of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I), 8.2 mol % of α-chloroacrylic acid-norbornane lactone units as monomer units (II), and 44.5 mol % of α-methylstyrene units as monomer units (III).

[0120] Example 9 Various operations, measurements and evaluations were carried out in the same manner as in Example 1, except that in the preparation of a copolymer, instead of the monomer composition A1, a monomer composition A9 containing 3.42 g of 1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl α-chloroacrylate (ACAFPh) as the monomer (a), 0.31 g of methyl α-chloroacrylate (ACAM) as the monomer (b), 2.28 g of α-methylstyrene (AMS) as the monomer (c), 0.00011 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as the polymerization initiator, and 3.97 g of cyclopentanone as the solvent was prepared. The results are shown in Table 1. The obtained copolymer A9 was a polymer containing 44.2 mol % of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I), 9.2 mol % of α-chloroacrylate methyl units as monomer units (II), and 46.6 mol % of α-methylstyrene units as monomer units (III).

[0121] Example 10 In the preparation of a copolymer, various operations, measurements and evaluations were carried out in the same manner as in Example 1, except that a monomer composition A10 containing 5.98 g of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl (ACAFPh) as the monomer (a), 0.38 g of α-chloroacrylic acid-gamma butyrolactone (ACAGBL) as the monomer (b), 3.54 g of α-methylstyrene (AMS) as the monomer (c), 0.00017 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as the polymerization initiator, and 6.72 g of cyclopentanone as the solvent was prepared instead of the monomer composition A1. The results are shown in Table 1. The obtained copolymer A10 was a copolymer containing 46.1 mol % of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I), 4.8 mol % of α-chloroacrylic acid-gamma butyrolactone units as monomer units (II), and 49.1 mol % of α-methylstyrene units as monomer units (III).

[0122] Example 11 In the preparation of a polymer, various operations, measurements and evaluations were carried out in the same manner as in Example 1, except that in place of the monomer composition A1, a monomer composition A11 containing 3.25 g of 1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl α-chloroacrylate (ACAFPh) as the monomer (a), 0.46 g of α-chloroacrylic acid-gamma butyrolactone (ACAGBL) as the monomer (b), 2.16 g of α-methylstyrene (AMS) as the monomer (c), 0.00011 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as the polymerization initiator, and 4.12 g of cyclopentanone as the solvent was prepared. The results are shown in Table 1. The obtained copolymer A11 was a polymer containing 47.2 mol % of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I), 8.5 mol % of α-chloroacrylic acid-gamma butyrolactone units as monomer units (II), and 44.3 mol % of α-methylstyrene units as monomer units (III).

[0123] Example 12 In the preparation of a copolymer, various operations, measurements and evaluations were carried out in the same manner as in Example 4, except that in place of the monomer composition A4, a monomer composition A12 containing 10.22 g of α-chloroacrylic acid-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl (ACAFPh) as the monomer (a), 0.65 g of α-chloroacrylic acid-norbornane lactone (ACAGBL) as the monomer (b), 6.03 g of α-methylstyrene (AMS) as the monomer (c), and 0.169 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as the polymerization initiator was prepared. The results are shown in Table 1. The obtained polymer A12 was a polymer containing 50.8 mol % of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I), 2.4 mol % of α-chloroacrylic acid-gamma butyrolactone units as monomer units (II), and 46.8 mol % of α-methylstyrene units as monomer units (III).

[0124] Comparative Example 1 Various operations, measurements and evaluations were carried out in the same manner as in Example 1, except that in the preparation of a copolymer, instead of the monomer composition A1, a monomer composition A13 containing 11.07 g of 1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl α-chloroacrylate (ACAFPh) as the monomer (a), 3.93 g of α-methylstyrene (AMS) as the monomer (c), 0.012 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as the polymerization initiator, and 8.73 g of cyclopentanone as the solvent was prepared. The results are shown in Table 1. The obtained copolymer A13 was a polymer containing 51.6 mol % of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I) and 48.4 mol % of α-methylstyrene units as monomer units (III).

[0125] Comparative Example 2 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the copolymer, instead of the monomer composition A1, a monomer composition A14 containing 2.70 g of 2-adamantyl α-chloroacrylate (ACA2Ad) as the monomer (b), 5.30 g of α-methylstyrene (AMS) as the monomer (c), 0.0019 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as the polymerization initiator, and 4.99 g of cyclopentanone as the solvent was prepared. The results are shown in Table 1. A resist formed using the obtained copolymer A14 could not be developed, and no resist pattern was obtained. Therefore, it was not possible to evaluate the exposure margin and the shape pattern. The obtained copolymer A14 was a polymer containing 52.0 mol % of α-chloroacrylate-2-adamantyl units as monomer units (II) and 48.0 mol % of α-methylstyrene units as monomer units (III).

[0126] Comparative Example 3 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the copolymer, instead of the monomer composition A1, a monomer composition A15 containing 3.36 g of α-chloroacrylic acid-norbornane lactone (ACANBL) as the monomer (b), 1.64 g of α-methylstyrene (AMS) as the monomer (c), 0.0051 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as the polymerization initiator, and 2.83 g of cyclopentanone as the solvent was prepared. The results are shown in Table 1. A resist formed using the obtained copolymer A15 could not be developed, and no resist pattern was obtained. Therefore, it was not possible to evaluate the exposure margin and the shape pattern. Furthermore, the copolymer A15 was not soluble in tetrahydrofuran, and therefore it was not possible to measure the molecular weight by gel permeation chromatography. The obtained copolymer A15 was a polymer containing 57.4 mol % of α-chloroacrylic acid-norbornane lactone units as monomer units (II) and 42.6 mol % of α-methylstyrene units as monomer units (III).

[0127] Comparative Example 4 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the copolymer, instead of the monomer composition A1, a monomer composition A16 containing 7.57 g of methyl α-chloroacrylate (ACAM) as the monomer (b), 7.43 g of α-methylstyrene (AMS) as the monomer (c), 0.023 g of V-601 (dimethyl 2,2'-azobis(2-methylpropionate) as the polymerization initiator, and 7.60 g of cyclopentanone as the solvent was prepared. The results are shown in Table 1. A resist formed using the obtained copolymer A16 could not be developed, and no resist pattern was obtained. Therefore, it was not possible to evaluate the exposure margin and the shape pattern. The obtained copolymer A16 was a polymer containing 58.3 mol % of methyl α-chloroacrylate units as monomer units (II) and 41.7 mol % of α-methylstyrene units as monomer units (III).

[0128] Comparative Example 5 In the preparation of the copolymer, various operations, measurements and evaluations were carried out in the same manner as in Example 1, except that in place of the monomer composition A1, a monomer composition A17 containing 3.48 g of 1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl α-chloroacrylate (ACAFPh) as the monomer (a), 2.52 g of 2-adamantyl α-chloroacrylate (ACA2Ad) as the monomer (b), 0.00048 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as the polymerization initiator, and 3.88 g of cyclopentanone as the solvent was prepared. The results are shown in Table 1. The obtained copolymer A17 was a polymer containing 51.0 mol % of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I) and 49.0 mol % of α-chloroacrylate-2-adamantyl units as monomer units (II).

[0129] Comparative Example 6 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the copolymer, instead of the monomer composition A1, a monomer composition A18 containing 3.47 g of 1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl α-chloroacrylate (ACAFPh) as the monomer (a), 2.53 g of norbornane lactone (ACANBL) as the monomer (b), 0.00048 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as the polymerization initiator, and 3.88 g of cyclopentanone as the solvent was prepared. The results are shown in Table 1. A resist formed using the obtained copolymer A18 could not be developed, and no resist pattern was obtained. Therefore, it was not possible to evaluate the exposure margin and the shape pattern. The obtained copolymer A18 was a polymer containing 43.0 mol % of α-chloroacrylic acid-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I) and 57.0 mol % of α-chloroacrylic acid-norbornane lactone units as monomer units (II).

[0130] Comparative Example 7 In the preparation of the copolymer, various operations, measurements and evaluations were carried out in the same manner as in Example 1, except that in place of the monomer composition A1, a monomer composition A19 containing 4.43 g of 1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl α-chloroacrylate (ACAFPh) as the monomer (a), 1.60 g of methyl α-chloroacrylate (ACAM) as the monomer (b), 0.00061 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as the polymerization initiator, and 3.80 g of cyclopentanone as the solvent was prepared. The results are shown in Table 1. The obtained copolymer A19 was a polymer containing 32.4 mol % of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I) and 67.6 mol % of α-chloroacrylate methyl units as monomer units (II).

[0131] Comparative Example 8 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the copolymer, instead of the monomer composition A1, a monomer composition A20 containing 2.66 g of α-chloroacrylic acid-gamma butyrolactone (ACAGBL) as the monomer (b), 1.65 g of α-methylstyrene (AMS) as the monomer (c), 0.0051 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as the polymerization initiator, and 3.63 g of cyclopentanone as the solvent was prepared. The results are shown in Table 1. A resist formed using the obtained copolymer A20 could not be developed, and no resist pattern was obtained. Therefore, it was not possible to evaluate the exposure margin and the shape pattern. Furthermore, the copolymer A20 was not soluble in tetrahydrofuran, and therefore it was not possible to measure the molecular weight by gel permeation chromatography. The obtained copolymer A20 was a polymer containing 55.8 mol % of α-chloroacrylic acid-gamma butyrolactone units as monomer units (II) and 44.2 mol % of α-methylstyrene units as monomer units (III).

[0132] Comparative Example 9 Various operations, measurements, and evaluations were carried out in the same manner as in Example 1, except that in the preparation of the copolymer, instead of the monomer composition A1, a monomer composition A21 containing 3.48 g of 1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl α-chloroacrylate (ACAFPh) as the monomer (a), 2.01 g of γ-chloroacrylic acid-gamma butyrolactone (ACAGBL) as the monomer (b), 0.00049 g of V-601 (dimethyl 2,2′-azobis(2-methylpropionate) as the polymerization initiator, and 4.50 g of cyclopentanone as the solvent was prepared. The results are shown in Table 1. A resist formed using the obtained copolymer A21 could not be developed, and no resist pattern was obtained. Therefore, it was not possible to evaluate the exposure margin and the shape pattern. The obtained copolymer A21 was a polymer containing 43.8 mol % of α-chloroacrylic acid-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units as monomer units (I) and 56.2 mol % of α-chloroacrylic acid-gamma butyrolactone units as monomer units (II).

[0133] In Table 1, "EB" represents an electron beam, "ACAFPh" represents an α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl unit, "ACAM" represents an α-chloroacrylate-methyl unit, "ACANBL" represents an α-chloroacrylic acid-norbornane lactone unit, "ACAGBL" represents an α-chloroacrylic acid-gamma butyrolactone unit, "ACA2Ad" represents an α-chloroacrylate-2-adamantyl unit, "AMS" represents an α-methylstyrene unit, and "IPA" represents isopropyl alcohol.

[0134] The results shown in Table 1 show that in Examples 1 to 12, which used copolymers containing the predetermined monomer units (I) to (III), a wide exposure margin was achieved and resist patterns with good shapes could be formed.

[0135] According to the present invention, it is possible to provide a copolymer and a positive resist composition which are capable of forming a resist pattern which has a wide exposure margin and a good shape, and also to provide a method of forming a resist pattern which is capable of forming a resist pattern which has a wide exposure margin and a good shape.

Claims

1. A compound represented by the following formula (I): (In formula (I), R 1 is a halogen atom or an alkyl group substituted with a halogen atom, R 2 is an organic group having a fluorine atom, R 3 and R 4 are hydrogen atoms, halogen atoms, unsubstituted alkyl groups or alkyl groups substituted with halogen atoms, and may be the same or different from each other. (In formula (II), R 5 is a halogen atom or an alkyl group substituted with a halogen atom, R 6 , R 7 and R 8 are hydrogen atoms or aliphatic groups which may have a substituent and do not have a fluorine atom, and may be the same or different from each other; R 6 , R 7 and R 8 may form a ring structure together with the carbon atom to which they are attached, R 9 and R 10 are hydrogen atoms or unsubstituted alkyl groups, and may be the same or different from each other; and a monomer unit (II) represented by the following formula (III): (In formula (III), R 11 and R 12 are hydrogen atoms or unsubstituted alkyl groups, which may be the same or different from each other; R 13 is an alkyl group which may have a substituent, R 14 is a halogen atom or an organic group, and p is an integer of 0 or more and 5 or less.

2. The above R 2 is a group represented by L-Ar (wherein L is a divalent linking group having a fluorine atom, and Ar is an aromatic ring group which may have a substituent).

3. The above R 6 , the R 7 and the R 8 The copolymer according to claim 1 , wherein is a hydrogen atom or an optionally substituted aliphatic group having 1 to 10 carbon atoms and no fluorine atom.

4. The copolymer according to claim 1, wherein the proportion of the monomer unit (II) is less than 30 mol %.

5. A positive resist composition comprising the copolymer according to any one of claims 1 to 4 and a solvent.

6. A method for forming a resist pattern, comprising the steps of: forming a resist film using the positive resist composition according to claim 5; exposing the resist film; and developing the exposed resist film.

7. The method for forming a resist pattern according to claim 6, wherein the development is carried out using an alcohol-based solvent.

Citation Information

Patent Citations

  • Polymer resin and preparation method thereof, electron beam photoresist and preparation and use method thereof

    CN113956395A

  • Preparation of fluoroalkyl alpha-chloroacrylate polymer or copolymer

    JP1986170735A

  • Resist pattern forming method

    JP2020052144A

  • Active light-sensitive or radiation-sensitive resin composition, resist film, method for forming pattern, and method for producing electronic device

    WO2024038802A1